Cover material, method for producing cover material, and laminate

The integration of a foamed vinyl chloride resin sheet with high branched poly(meth)acrylate content into the skin of automobile interior parts addresses the challenge of inadequate cushioning and thermal stability, resulting in enhanced performance and stability for these components.

WO2024203561A1PCT designated stage expired Publication Date: 2024-10-03ZEON CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010610
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-18
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current automobile interior parts skins lack optimal cushioning properties, particularly in high-temperature and high-pressure conditions, due to insufficient thermal stability and cushioning performance.

Method used

A skin composed of a vinyl chloride resin molded sheet with a foamed vinyl chloride resin molded sheet containing 10% or more branched poly(meth)acrylate monomer units, which enhances cushioning properties and suppresses thermal shrinkage when combined with a foamed polyurethane molded body.

Benefits of technology

The solution provides an epidermis with improved cushioning properties and thermal stability, suitable for use in automobile interior parts such as instrument panels and door trims, by fine-tuning the cell diameter of foamed cells and interposing the foamed vinyl chloride resin sheet between the vinyl chloride resin sheet and the polyurethane molded body.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

To provide a cover material having excellent cushioning properties. The present invention is a cover material having a vinyl chloride resin molded sheet (X) and a foamed vinyl chloride resin molded sheet (Y) disposed on one side of the vinyl chloride resin molded sheet (X) in the thickness direction, wherein: the vinyl chloride resin molded sheet (X) includes a vinyl chloride resin (a) and a plasticizer (b); the content of the plasticizer (b) in the vinyl chloride resin molding sheet (X) is 50 parts by mass or more with respect to 100 parts by mass of the vinyl chloride resin (a); the foamed vinyl chloride resin molded sheet (Y) contains a vinyl chloride resin (c) and a poly(meth)acrylate (d); and the poly(meth)acrylate (d) contains 10 mass% or more of a monomer unit derived from a (meth)acrylate which is a branched alkyl ester.
Need to check novelty before this filing date? Find Prior Art

Description

Surface skin, method for manufacturing surface skin and laminate

[0001] The present invention relates to a surface skin, a method for producing the surface skin, and a laminate.

[0002] Vinyl chloride resins are generally used in a variety of applications due to their excellent properties, such as cold resistance, heat resistance, oil resistance, etc. Specifically, for example, conventionally, automobile interior parts such as automobile instrument panels have been formed using automobile interior materials such as a skin made of a vinyl chloride resin molded product (hereinafter sometimes referred to as a "vinyl chloride resin molded sheet") obtained by molding a vinyl chloride resin composition into a sheet, or a laminate made by lining a foam such as polyurethane foam on the skin made of the vinyl chloride resin molded sheet.

[0003] For example, Patent Document 1 reports that a skin formed by placing a foamed vinyl chloride resin sheet on one thickness-wise side of a molded vinyl chloride resin sheet containing a predetermined amount of plasticizer can effectively suppress thermal shrinkage when a foamed polyurethane molded body is used as the backing. Also, Patent Document 2 reports that a skin formed by placing a foamed vinyl chloride resin sheet containing a vinyl chloride resin with an average degree of polymerization of a predetermined value or more and a density of a predetermined value or less on one thickness-wise side of a molded vinyl chloride resin sheet containing a predetermined amount of plasticizer can improve cushioning properties after high-temperature, high-pressure treatment.

[0004] International Publication No. 2019 / 188520 Japanese Patent Application Laid-Open No. 2021-133662

[0005] However, there is still a high demand for cushioning properties in the skins of automobile interior parts, and skins with excellent cushioning properties are still desired.

[0006] Therefore, an object of the present invention is to provide a surface skin having excellent cushioning properties, and a laminate having such a surface skin and having excellent cushioning properties.

[0007] The present inventors have conducted extensive research to solve the above-mentioned problems, and have found that a surface layer can exhibit excellent cushioning properties if it is formed by placing a foamed vinyl chloride resin molded sheet containing poly(meth)acrylate containing 10% by mass or more of monomer units derived from branched alkyl ester (meth)acrylate on one side in the thickness direction of a vinyl chloride resin molded sheet containing a predetermined amount of plasticizer, and have completed the present invention.

[0008] That is, the present invention has an object to advantageously solve the above-mentioned problems, and its gist is as follows: [1] A skin having a molded vinyl chloride resin sheet (X) and a foamed vinyl chloride resin molded sheet (Y) arranged on one side of the molded vinyl chloride resin sheet (X) in the thickness direction, wherein the molded vinyl chloride resin sheet (X) contains a vinyl chloride resin (a) and a plasticizer (b), the content of the plasticizer (b) in the molded vinyl chloride resin sheet (X) is 50 parts by mass or more per 100 parts by mass of the vinyl chloride resin (a), the foamed vinyl chloride resin molded sheet (Y) contains a vinyl chloride resin (c) and a poly(meth)acrylate (d), and the poly(meth)acrylate (d) contains 10% by mass or more of a monomer unit derived from a branched alkyl ester (meth)acrylate. [2] The skin of [1], wherein the poly(meth)acrylate (c) is at least one selected from homopolymers and copolymers of (meth)acrylates that are branched alkyl esters, or a combination of at least one selected from homopolymers and copolymers of (meth)acrylates that are branched alkyl esters and at least one selected from homopolymers and copolymers of (meth)acrylates that are linear alkyl esters. [3] The skin of [1] or [2], wherein the content of the poly(meth)acrylate (d) in the foamed vinyl chloride resin molded sheet (Y) is 0.01 parts by mass or more and 5.0 parts by mass or less per 100 parts by mass of the vinyl chloride resin (c). [4] The skin of any of [1] to [3], wherein the foamed vinyl chloride resin molded sheet (Y) further contains a plasticizer (e), and the content of the plasticizer (e) in the foamed vinyl chloride resin molded sheet (Y) is 50 parts by mass or more and 200 parts by mass or less per 100 parts by mass of the vinyl chloride resin (c). [5] The skin of any of [1] to [4], wherein the foamed vinyl chloride resin molded sheet (Y) further contains an azo compound, and the content of the azo compound in the foamed vinyl chloride resin molded sheet (Y) is 0.05 parts by mass or more and 1.00 parts by mass or less per 100 parts by mass of the vinyl chloride resin (c). [6] The skin of any of [1] to [5], wherein the foamed vinyl chloride resin molded sheet (Y) has a thickness of 1.5 mm or more.[7] The skin according to any one of [1] to [6], which is for use in the skin of an automobile interior part. [8] A method for producing a skin having a molded vinyl chloride resin sheet (X) and a foamed vinyl chloride resin molded sheet (Y), the method comprising: a first step of forming the molded vinyl chloride resin sheet (X) using a vinyl chloride resin composition (A) containing a vinyl chloride resin (a) and a plasticizer (b); and a second step of forming the foamed vinyl chloride resin molded sheet (Y) on one side in the thickness direction of the molded vinyl chloride resin sheet (X) using an expandable vinyl chloride resin composition (B), wherein the content of the plasticizer (b) in the vinyl chloride resin composition (A) is 50 parts by mass or more per 100 parts by mass of the vinyl chloride resin (a), the foamed vinyl chloride resin molded sheet (Y) contains a vinyl chloride resin (c) and a poly(meth)acrylate (d), and the poly(meth)acrylate (d) contains 10% by mass or more of a monomer unit derived from a branched alkyl ester (meth)acrylate. [9] A laminate comprising a foamed polyurethane molded body and a surface skin according to any one of [1] to [7], wherein the foamed vinyl chloride resin molded sheet (Y) is disposed between the foamed polyurethane molded body and the foamed vinyl chloride resin molded sheet (X).

[0009] According to the present invention, it is possible to provide a surface skin having excellent cushioning properties. Furthermore, according to the present invention, it is possible to provide a laminate having the surface skin and having excellent cushioning properties.

[0010] Hereinafter, embodiments of the present invention will be described in detail. The skin of the present invention can be used, for example, to produce the laminate of the present invention. The skin of the present invention can be suitably used, for example, as an automobile interior material, such as the skin of an automobile interior part, such as an automobile instrument panel or door trim. The skin of the present invention can be produced by the method for producing a skin of the present invention.

[0011] (Surface) The surface of the present invention includes a molded vinyl chloride resin sheet (X) containing a predetermined amount of plasticizer and a foamed vinyl chloride resin sheet (Y) arranged on one side of the molded vinyl chloride resin sheet (X) in the thickness direction, wherein the foamed vinyl chloride resin sheet (Y) contains a poly(meth)acrylate (d) containing 10% by mass or more of a monomer unit derived from a branched alkyl ester (meth)acrylate. Hereinafter, "branched alkyl ester (meth)acrylate" may be referred to as "branched (meth)acrylate." Furthermore, "monomer unit derived from a branched alkyl ester (meth)acrylate" may be referred to as "branched (meth)acrylate monomer unit." In this specification, "(meth)acrylate" refers to acrylate and / or methacrylate. In this specification, "poly(meth)acrylate" refers to a polymer containing (meth)acrylate as a monomer, and the monomer unit constituting the polymer is derived from (meth)acrylate. By incorporating a branched poly(meth)acrylate into the foamed vinyl chloride resin molded sheet (Y), the cell diameter of the foam cells (air bubbles) in the foamed vinyl chloride resin molded sheet (Y) can be made finer, resulting in a surface with excellent cushioning properties.

[0012] In the skin of the present invention, the foamed vinyl chloride resin molded sheet (Y) is disposed on one side of the foamed vinyl chloride resin molded sheet (X) in the thickness direction, and therefore, when a foamed polyurethane molded product is used as a backing, i.e., when a foamed polyurethane molded product is further laminated on the side where the foamed vinyl chloride resin molded sheet (Y) is disposed, thermal shrinkage can be effectively suppressed.

[0013] The skin of the present invention is suitably used as an automobile interior member, for example, as the skin of an automobile interior part such as an automobile instrument panel or door trim, and is particularly suitably used as the skin of an automobile instrument panel.

[0014] <Vinyl chloride resin molded sheet (X)> The vinyl chloride resin molded sheet (X) is obtained by molding a vinyl chloride resin composition (A) containing a vinyl chloride resin and a predetermined amount of a plasticizer into a sheet. Note that the vinyl chloride resin molded sheet (X) is usually not a foam, unlike the foamed vinyl chloride resin molded sheet (Y) described below.

[0015] The thickness of the vinyl chloride resin molded sheet (X) is not particularly limited, but is preferably 0.1 mm or more, more preferably 0.5 mm or more, even more preferably 0.7 mm or more, and preferably 5.0 mm or less, more preferably 2.0 mm or less, even more preferably 1.8 mm or less, and even more preferably 1.5 mm or less. If the thickness of the vinyl chloride resin molded sheet (X) is equal to or greater than the above-mentioned lower limit, the resulting vinyl chloride resin molded sheet (X) can be imparted with good tensile elongation at low temperatures. Furthermore, if the thickness of the vinyl chloride resin molded sheet (X) is equal to or less than the above-mentioned upper limit, the resulting vinyl chloride resin molded sheet (X) is easy to handle, and it is easier to arrange a foamed vinyl chloride resin molded sheet (Y) on the vinyl chloride resin molded sheet (X). The thickness of the vinyl chloride resin molded sheet (X) can be measured using an optical microscope.

[0016] <<Vinyl chloride resin composition (A)>> The vinyl chloride resin composition (A) contains a vinyl chloride resin (a) and a predetermined amount of a plasticizer (b), and may further contain various additives, etc. The content of each component in the vinyl chloride resin composition (A) relative to the vinyl chloride resin (a) is the same as the content of each component in the vinyl chloride resin molded sheet (X) relative to the vinyl chloride resin (a), excluding components that can be decomposed during the molding process.

[0017] [Vinyl chloride resin (a)] The vinyl chloride resin (a) contained in the vinyl chloride resin composition (A) may contain, for example, one or more types of vinyl chloride resin particles, and may optionally further contain one or more types of vinyl chloride resin microparticles. Among these, the vinyl chloride resin (a) preferably contains at least vinyl chloride resin particles, and more preferably contains vinyl chloride resin particles and vinyl chloride resin microparticles.

[0018] In this specification, "resin particles" refers to particles having a particle diameter of 30 μm or more, and "resin fine particles" refers to particles having a particle diameter of less than 30 μm. Vinyl chloride resin particles usually function as a matrix resin (base material), and vinyl chloride resin fine particles usually function as a dusting agent (powder flowability improver).

[0019] The vinyl chloride resin (a) can be produced by any conventionally known production method, such as suspension polymerization, emulsion polymerization, solution polymerization, bulk polymerization, etc. Vinyl chloride resin particles are preferably produced by suspension polymerization, and vinyl chloride resin microparticles are preferably produced by emulsion polymerization.

[0020] -Composition- Examples of the vinyl chloride resin (a) include homopolymers composed of vinyl chloride monomer units, as well as vinyl chloride copolymers containing preferably 50% by mass or more, more preferably 70% by mass or more, of vinyl chloride monomer units. Specific examples of monomers (comonomers) copolymerizable with vinyl chloride monomers that can constitute the vinyl chloride copolymers include olefins such as ethylene and propylene; halogenated olefins such as allyl chloride, vinylidene chloride, vinyl fluoride, and trifluorochloroethylene; vinyl carboxylic acid esters such as vinyl acetate and vinyl propionate; vinyl ethers such as isobutyl vinyl ether and cetyl vinyl ether; allyl ethers such as allyl-3-chloro-2-oxypropyl ether and allyl glycidyl ether; acrylic acid, maleic acid, itaconic acid, acrylic acid Examples of the comonomer include unsaturated carboxylic acids, esters, and anhydrides thereof, such as 2-hydroxyethyl acrylate, methyl methacrylate, monomethyl maleate, diethyl maleate, and maleic anhydride; unsaturated nitriles, such as acrylonitrile and methacrylonitrile; acrylamides, such as acrylamide, N-methylolacrylamide, acrylamido-2-methylpropanesulfonic acid, and (meth)acrylamidopropyltrimethylammonium chloride; and allylamines and derivatives thereof, such as allylamine benzoate and diallyldimethylammonium chloride. The above-listed monomers are only a partial list of possible comonomers, and various monomers listed in "Polyvinyl Chloride," edited by the Kinki Chemical Association Vinyl Division, published by Nikkan Kogyo Shimbun, pp. 75-104 (1988), can also be used as the comonomer. These comonomers may be used alone or in combination of two or more. The vinyl chloride resin also includes resins obtained by graft-polymerizing (1) vinyl chloride or (2) vinyl chloride with the above-mentioned comonomer onto a resin such as an ethylene-vinyl acetate copolymer, an ethylene-methyl methacrylate copolymer, an ethylene-ethyl acrylate copolymer, or a chlorinated polyethylene.

[0021] -Average Degree of Polymerization- The average degree of polymerization of the vinyl chloride resin (a) is not particularly limited, but is preferably 1200 or more, more preferably 1300 or more, even more preferably 1400 or more, and even more preferably 1500 or more, and is preferably 3000 or less, more preferably 2500 or less, and even more preferably 2000 or less. If the average degree of polymerization of the vinyl chloride resin (a) is equal to or greater than the above-mentioned lower limit, the vinyl chloride resin (a) has an appropriate hardness, which is advantageous in that it improves the strength of the vinyl chloride resin molded sheet (X) and enhances the cushioning properties of the surface. On the other hand, if the average degree of polymerization of the vinyl chloride resin (a) is equal to or less than the above-mentioned upper limit, the vinyl chloride resin (a) has an appropriate flexibility, which makes it easy to mold the vinyl chloride resin composition (A) into the vinyl chloride resin molded sheet (X). In this specification, the average degree of polymerization of the vinyl chloride resin can be measured by a method in accordance with JIS K6720-2.

[0022] [Plasticizer (b)] The vinyl chloride resin composition (A) further contains a predetermined amount of plasticizer (b). If the vinyl chloride resin composition (A) does not contain the plasticizer (b), it will be impossible to satisfactorily obtain a vinyl chloride resin molded sheet (X) using the vinyl chloride resin composition (A).

[0023] -Content- The content of the plasticizer (b) must be 50 parts by mass or more, preferably 55 parts by mass or more, more preferably 60 parts by mass or more, even more preferably 65 parts by mass or more, even more preferably 70 parts by mass or more, even more preferably 85 parts by mass or more, and is preferably 200 parts by mass or less, more preferably 170 parts by mass or less, even more preferably 140 parts by mass or less, and even more preferably 100 parts by mass or less, per 100 parts by mass of the vinyl chloride resin (a). If the content of the plasticizer (b) is at or above the above-mentioned lower limit, it imparts excellent flexibility to the vinyl chloride resin composition (A), for example, making it easier to process into a vinyl chloride resin molded sheet (X), and is advantageous in terms of imparting cushioning properties to the resulting vinyl chloride resin molded sheet (X). Furthermore, if the content of the plasticizer (b) is at or below the above-mentioned upper limit, it is possible to suppress stickiness on the surface of the resulting vinyl chloride resin molded sheet (X) and improve surface slipperiness.

[0024] -Type- As the plasticizer (b), for example, the primary plasticizers and secondary plasticizers described in International Publication No. 2016 / 098344 can be used. These components may be used alone, or two or more may be used in combination in any ratio. Among the plasticizers described above, from the viewpoint of easily and satisfactorily obtaining the vinyl chloride resin composition (A) and the vinyl chloride resin molded sheet (X), it is preferable to use at least a primary plasticizer as the plasticizer (b), and it is more preferable to use a primary plasticizer and a secondary plasticizer in combination. Specifically, it is preferable to use a trimellitic acid ester and / or a pyromellitic acid ester as the plasticizer (b), it is more preferable to use at least a trimellitic acid ester, and it is even more preferable to use a trimellitic acid ester in combination with epoxidized soybean oil.

[0025] [Additives] In addition to the components described above, the vinyl chloride resin composition (A) may further contain various additives. Examples of additives include, but are not limited to, stabilizers such as perchloric acid-treated hydrotalcite, zeolite, β-diketone, and fatty acid metal salts; mold release agents; dusting agents other than the vinyl chloride resin fine particles; impact resistance modifiers; perchloric acid compounds other than perchloric acid-treated hydrotalcite (e.g., sodium perchlorate and potassium perchlorate); antioxidants; mildew inhibitors; flame retardants; antistatic agents; fillers; light stabilizers; moldability adjusters (e.g., silicone oil); and colorants. Examples of such additives include, but are not limited to, those described in WO 2016 / 098344 (excluding foaming agents). The content of the various additives in the vinyl chloride resin composition (A) can be adjusted as appropriate within a range in which the desired effects of the present invention are achieved.

[0026] [Method for Preparing Vinyl Chloride Resin Composition (A)] The vinyl chloride resin composition (A) can be prepared by mixing the above-mentioned components without any particular limitation. The method for mixing the vinyl chloride resin (a), a predetermined amount of plasticizer (b), and various additives further used as needed is not particularly limited, and examples thereof include a method in which the components excluding the dusting agent containing vinyl chloride resin fine particles are mixed by dry blending, and then the dusting agent is added and mixed. A Henschel mixer is preferably used for dry blending. The temperature during dry blending is not particularly limited, and is preferably 50°C or higher, more preferably 70°C or higher, and preferably 200°C or lower.

[0027] <Foamed vinyl chloride resin molded sheet (Y)> The skin of the present invention comprises a foamed vinyl chloride resin molded sheet (Y) containing poly(meth)acrylate (d) disposed on one side in the thickness direction of the above-mentioned foamed vinyl chloride resin molded sheet (X), where the poly(meth)acrylate (d) contains 10% by mass or more of a branched (meth)acrylate monomer unit. The content of poly(meth)acrylate (d) and the content of each monomer unit in the foamed vinyl chloride resin molded sheet (Y) can be calculated from the monomer composition in the composition used for sheet molding. Alternatively, the sheet (Y) can be dissolved in THF and filtered. A poor solvent is added to the filtrate to precipitate the polymer, followed by centrifugation and drying to separate the polymer component. The amount of vinyl chloride resin is then determined by quantifying the amount of chlorine using ion chromatography or titration, and the amount is subtracted from the total to determine the (meth)acrylate content. The branched to linear ratio of poly(meth)acrylate (d) is calculated as follows: 1 It can be measured using a nuclear magnetic resonance (NMR) method such as H-NMR.

[0028] The foamed vinyl chloride resin molded sheet (Y) is preferably located on one surface in the thickness direction of the skin of the present invention. Note that the one surface in the thickness direction of the skin of the present invention may be partially or entirely composed of the foamed vinyl chloride resin molded sheet (Y).

[0029] It is generally believed that when a skin made of a vinyl chloride resin molded sheet containing a plasticizer is placed under high-temperature conditions in direct contact with a urethane foam molded body, for example, the plasticizer in the skin migrates to the urethane foam molded body, reducing the amount of plasticizer in the skin and causing thermal shrinkage of the skin. However, in the skin of the present invention, which is made by disposing a foamed vinyl chloride resin sheet (Y) on one side in the thickness direction of a plasticizer-containing vinyl chloride resin molded sheet (X), interposing the foamed vinyl chloride resin sheet (Y) between the vinyl chloride resin molded sheet (X) and the urethane foam molded body makes it difficult for the plasticizer to migrate from the vinyl chloride resin molded sheet (X) and the foamed vinyl chloride resin molded sheet (Y) to reach the urethane foam molded body, which is advantageous in suppressing thermal shrinkage.

[0030] The foamed vinyl chloride resin molded sheet (Y) may be directly bonded to the vinyl chloride resin molded sheet (X), or may be bonded to the vinyl chloride resin molded sheet (X) via another resin layer or the like, as long as the desired effect is obtained. However, from the viewpoint of further suppressing thermal shrinkage when a urethane foam molded body is used as the surface backing, it is preferable that the foamed vinyl chloride resin molded sheet (Y) be directly bonded to the vinyl chloride resin molded sheet (X).

[0031] The density of the foamed vinyl chloride resin molded sheet (Y) is 0.50 g / cm 3 Preferably, it is 0.40 g / cm or less. 3 More preferably, it is 0.35 g / cm or less. 3 More preferably, it is 0.25 g / cm or less. 3 It is more preferable that the viscosity is 0.10 g / cm or less. 3 It is preferable that the density is 0.12 g / cm or more. 3 More preferably, it is 0.15 g / cm or more. 3 It is even more preferable that the density of the foamed vinyl chloride resin molded sheet (Y) is within the above range, which is advantageous in that cushioning properties can be improved by using the foamed vinyl chloride resin molded sheet (Y). The density of the foamed vinyl chloride resin molded sheet (Y) can be adjusted by the type and amount of the foaming agent in the foamable vinyl chloride resin composition (Y) described below, and by conditions such as the temperature when the foamable vinyl chloride resin composition (Y) is molded into the foamed vinyl chloride resin molded sheet (Y).

[0032] The thickness of the foamed vinyl chloride resin molded sheet (Y) is not particularly limited, but is preferably 1.5 mm or more, more preferably 1.8 mm or more, even more preferably 2.0 mm or more, even more preferably 2.3 mm or more, and even more preferably 2.5 mm or more, and is preferably 10.0 mm or less, and more preferably 5.0 mm or less. If the thickness of the foamed vinyl chloride resin molded sheet (Y) is equal to or greater than the above-mentioned lower limit, when the resulting skin is used to back a foamed polyurethane molded article, thermal shrinkage of the skin can be further suppressed, and the hardness of the skin can be reduced, which is advantageous in improving cushioning properties. On the other hand, if the thickness of the foamed vinyl chloride resin molded sheet (Y) is equal to or less than the above-mentioned upper limit, the resulting skin will be easy to handle when backing a foamed polyurethane molded article.

[0033] The foamed vinyl chloride resin molded sheet (Y) is not particularly limited, but is usually obtained by foaming the foamable vinyl chloride resin composition (B) and molding it into a sheet. The foaming ratio can be, for example, 3.0 to 6.0, preferably 3.5 or more and 5.5 or less. The foaming ratio can be determined by dividing the density of the foamed vinyl chloride resin molded sheet (Y) by the density of a sheet molded in the same manner as the foamed vinyl chloride resin molded sheet (Y) but without a foaming agent.

[0034] <<Expandable Vinyl Chloride Resin Composition (B)>> The expandable vinyl chloride resin composition (B) contains a vinyl chloride resin (c), a poly(meth)acrylate (d), and a foaming agent, and may optionally further contain a plasticizer (e), other polymers, various additives, and the like.

[0035] It should be noted that, except for components that can be decomposed during the molding process, such as the thermally decomposable foaming agent described below, the content of each component in the expandable vinyl chloride resin composition (B) relative to the vinyl chloride resin is the same as the content of each component in the foamed vinyl chloride resin molded product (Y) relative to the vinyl chloride resin.

[0036] [Vinyl chloride resin (c)] The vinyl chloride resin (c) contained in the expandable vinyl chloride resin composition (B) may contain, for example, one or more types of vinyl chloride resin particles, and may optionally further contain one or more types of vinyl chloride resin microparticles. Among these, the vinyl chloride resin (a) preferably contains at least vinyl chloride resin particles, and more preferably contains vinyl chloride resin particles and vinyl chloride resin microparticles.

[0037] The vinyl chloride resin particles usually function as a matrix resin (base material), and the vinyl chloride resin fine particles usually function as a dusting agent (powder flowability improver).

[0038] The vinyl chloride resin (c) can be produced by any conventionally known production method, such as suspension polymerization, emulsion polymerization, solution polymerization, bulk polymerization, etc. The vinyl chloride resin particles are preferably produced by suspension polymerization, and the vinyl chloride resin microparticles are preferably produced by emulsion polymerization.

[0039] As the vinyl chloride resin (c), for example, a polymer that can be used as the vinyl chloride resin (a) in the vinyl chloride resin composition (A) described above in the section "Vinyl chloride resin molded sheet (X)" can be used.

[0040] The average degree of polymerization of the vinyl chloride resin (c) is preferably 1200 or more, more preferably 1300 or more, even more preferably 1400 or more, and even more preferably 1500 or more, and is preferably 3000 or less, more preferably 2500 or less, and even more preferably 2000 or less. If the average degree of polymerization of the vinyl chloride resin (c) is equal to or greater than the above-mentioned lower limit, it is advantageous in that the cushioning properties of the surface can be enhanced. On the other hand, if the average degree of polymerization of the vinyl chloride resin (c) is equal to or less than the above-mentioned upper limit, the vinyl chloride resin (c) has an appropriate flexibility, which is advantageous in that it is easy to mold the foamable vinyl chloride resin composition (B) into a foamed vinyl chloride resin molded sheet (Y) and that the cushioning properties of the surface can be enhanced.

[0041] [Blowing Agent] The expandable vinyl chloride resin composition (B) contains a blowing agent. By including a blowing agent in the expandable vinyl chloride resin composition (B), the expandable vinyl chloride resin composition (B) can be molded while being foamed to obtain a foamed vinyl chloride resin molded sheet (Y) in a good condition. The blowing agent contained in the expandable vinyl chloride resin composition (B) can be a chemical blowing agent, a physical blowing agent, or the like.

[0042] Examples of chemical foaming agents include thermal decomposition type foaming agents and reactive type foaming agents.

[0043] Examples of the thermally decomposable foaming agent that can be used include organic thermally decomposable foaming agents such as azo compounds, nitroso compounds, hydrazine derivatives, semicarbazide compounds, tetrazole compounds, and organic acids; and inorganic thermally decomposable foaming agents such as bicarbonates, carbonates, organic acid salts, and nitrites.

[0044] Examples of azo compounds include azodicarbonamide (ADCA), azobisisobutyronitrile (AIBN), barium azodicarboxylate, and diazoaminobenzene. Examples of nitroso compounds include dinitrosopentamethylenetetramine (DPT). Examples of hydrazine derivatives include p,p'-oxybis(benzenesulfonylhydrazide) (OBSH), paratoluenesulfonylhydrazide (TSH), and hydrazodicarbonamide (HDCA). Examples of semicarbazide compounds include p-toluenesulfonylsemicarbazide. Examples of tetrazole compounds include 5-phenyltetrazole and 1,4-bistetrazole. Examples of organic acids include polycarboxylic acids such as citric acid, oxalic acid, fumaric acid, phthalic acid, malic acid, and tartaric acid.

[0045] Examples of reactive foaming agents include a combination of an isocyanate compound and water, a combination of sodium bicarbonate and acid, a combination of hydrogen peroxide and yeast, and a combination of zinc powder and acid.

[0046] Examples of physical foaming agents include gases such as chlorofluorocarbons and carbon dioxide; volatile liquids such as water and volatile hydrocarbon compounds; and thermally expandable microcapsules encapsulating these gases, volatile liquids, etc.

[0047] Among the foaming agents mentioned above, it is preferable to use a thermally decomposable foaming agent, more preferably an azo compound, and particularly preferably azodicarbonamide (ADCA). When a thermally decomposable foaming agent is used as the foaming agent, the foamed vinyl chloride resin molded sheet (Y) can be molded while the foamable vinyl chloride resin composition (B) is foamed well, so that when the resulting skin is backed with a foamed polyurethane molded body and used, thermal shrinkage can be more effectively suppressed and the cushioning properties of the skin can be further improved. Furthermore, when an azo compound is used as the thermally decomposable foaming agent, the foamed vinyl chloride resin molded sheet (Y) can be molded while the foamable vinyl chloride resin composition (B) is foamed well, so that when the resulting skin is backed with a foamed polyurethane molded body and used, thermal shrinkage can be more effectively suppressed and the cushioning properties of the skin can be further improved.

[0048] The volume average particle diameter of the thermal decomposition type foaming agent is preferably 30 μm or less, more preferably 20 μm or less, even more preferably 10 μm or less, even more preferably 7 μm or less, even more preferably 5 μm or less, even more preferably 4 μm or less, most preferably 3 μm or less, and preferably 1 μm or more. When the volume average particle diameter of the thermal decomposition type foaming agent is equal to or less than the upper limit, the expansion ratio of the foamable vinyl chloride resin composition (B) can be improved, the hardness of the resulting skin can be reduced, and cushioning properties can be further enhanced. On the other hand, when the volume average particle diameter of the thermal decomposition type foaming agent is equal to or greater than the lower limit, the thermal decomposition type foaming agent can be easily handled. In this specification, the term "volume average particle diameter" refers to the particle diameter (median diameter) at which the cumulative volume calculated from the smallest diameter side becomes 50% in the particle size distribution (volume basis) measured using a laser diffraction / scattering type particle size distribution analyzer.

[0049] The content of the thermally decomposable foaming agent in the expandable vinyl chloride resin composition (B) is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and even more preferably 3 parts by mass or more, per 100 parts by mass of the vinyl chloride resin. It is also preferably 10 parts by mass or less, more preferably 5 parts by mass or less, and even more preferably 4 parts by mass or less. When the content of the thermally decomposable foaming agent is equal to or greater than the lower limit, the expansion ratio of the expandable vinyl chloride resin composition (B) is improved, the hardness of the resulting skin is reduced, and cushioning properties are further enhanced. On the other hand, when the content of the thermally decomposable foaming agent is equal to or less than the upper limit, the uniformity of the foam cells (bubbles) is improved, and the hardness of the resulting skin is reduced substantially uniformly regardless of location, and cushioning properties are further enhanced.

[0050] When a thermally decomposable foaming agent is used as the foaming agent in the foamable vinyl chloride resin composition (B), at least a portion of the thermally decomposable foaming agent decomposes when the foamable vinyl chloride resin composition (B) is used to form the foamed vinyl chloride resin molded sheet (Y), and the thermally decomposable foaming agent may be contained as a residue in the resulting foamed vinyl chloride resin molded sheet (Y). For example, when an azo compound is used as the thermally decomposable foaming agent, the content (residual amount) of the azo compound in the foamed vinyl chloride resin molded sheet (Y) formed is preferably 0.05 parts by mass or more, more preferably 0.10 parts by mass or more, and even more preferably 0.20 parts by mass or more, and preferably 1.00 parts by mass or less, more preferably 0.75 parts by mass or less, and even more preferably 0.50 parts by mass or less, per 100 parts by mass of the vinyl chloride resin (c). If the content (residual amount) of the azo compound in the foamed vinyl chloride resin molded sheet (Y) is equal to or greater than the above-mentioned lower limit, the flexibility of the foamed vinyl chloride resin molded sheet (Y) can be appropriately improved, which is advantageous in that it can enhance cushioning properties. On the other hand, if the content (residual amount) of the azo compound in the foamed vinyl chloride resin molded sheet (Y) is equal to or less than the above-mentioned upper limit, the flexibility of the foamed vinyl chloride resin molded sheet (Y) can be prevented from becoming excessively high, and the strength of the foam cells (air bubbles) can be increased. This is advantageous in that it can enhance cushioning properties of a skin having the foamed vinyl chloride resin molded sheet (Y).

[0051] [Poly(meth)acrylate (d)] The foamable vinyl chloride resin composition (B) contains a poly(meth)acrylate (d) containing 10% by mass or more of a monomer unit derived from a branched alkyl ester (meth)acrylate. By including such a poly(meth)acrylate (d) in the foamable vinyl chloride resin composition (B), the cell diameter of the foam cells (air bubbles) in the foamed vinyl chloride resin molded sheet (Y) can be made finer, resulting in a surface with excellent cushioning properties.

[0052] The branched (meth)acrylate monomer units in the poly(meth)acrylate (d) are preferably 12% by mass or more, more preferably 14% by mass or more, from the viewpoint of the expression of the effects of the branched (meth)acrylate monomer units. The branched (meth)acrylate monomer units may be 100% by mass. Examples of monomer units other than the branched (meth)acrylate monomer units include monomer units derived from a linear alkyl ester (meth)acrylate (hereinafter also referred to as "linear (meth)acrylate") (hereinafter also referred to as "linear (meth)acrylate monomer units").

[0053] When linear (meth)acrylate monomer units are used in combination, the linear (meth)acrylate monomer units are preferably 15% by mass or more, more preferably 20% by mass or more, in order to fully obtain the combined effect. Furthermore, when used in combination, the linear (meth)acrylate monomer units can be 90% by mass or less, preferably 88% by mass or less, more preferably 86% by mass or less, in order to fully obtain the effect of the branched (meth)acrylate monomer units. Poly(meth)acrylate (d) can be composed of branched (meth)acrylate monomer units and linear (meth)acrylate monomer units.

[0054] The poly(meth)acrylate (d) may be composed of one type of poly(meth)acrylate or two or more types of poly(meth)acrylates. The poly(meth)acrylate (d) may be a homopolymer of one type of (meth)acrylate or a copolymer of two or more types of (meth)acrylates.

[0055] When the poly(meth)acrylate (d) is one type of poly(meth)acrylate, examples of the poly(meth)acrylate (d) include a homopolymer of one type of branched (meth)acrylate; a copolymer of two or more types of branched (meth)acrylate; and a copolymer of one or more types of branched (meth)acrylate and one or more types of linear (meth)acrylate. From the viewpoint of uniformity of foam cells (bubbles), a homopolymer of one type of branched (meth)acrylate and a copolymer of two or more types of branched (meth)acrylate are preferred, and a homopolymer of one type of branched (meth)acrylate is more preferred. In this case, all monomer units are monomer units derived from the branched (meth)acrylate.

[0056] When the poly(meth)acrylate (d) is two or more types of poly(meth)acrylates, the combination of the two or more types of poly(meth)acrylates is not particularly limited as long as the proportion of branched (meth)acrylate-derived monomer units among all monomer units constituting the two or more types of poly(meth)acrylates is 10 mass% or more. All of the poly(meth)acrylates of the two or more types of poly(meth)acrylates may have branched (meth)acrylate monomer units, or some of the poly(meth)acrylates may have branched (meth)acrylate monomer units, and the remaining poly(meth)acrylates may not have branched (meth)acrylate monomer units.

[0057] When the poly(meth)acrylate (d) is two or more types of poly(meth)acrylate, the poly(meth)acrylate (d) may be a combination of two or more types of homopolymers of branched (meth)acrylate; a combination of at least one type selected from homopolymers and copolymers of branched (meth)acrylate with at least one type selected from homopolymers and copolymers of linear (meth)acrylate; a combination of two or more types of copolymers of branched (meth)acrylate and linear (meth)acrylate; a copolymer of branched (meth)acrylate and linear (meth)acrylate; and a combination of at least one selected from homopolymers and copolymers of branched (meth)acrylate; a combination of a copolymer of branched (meth)acrylate and linear (meth)acrylate with at least one selected from homopolymers and copolymers of linear (meth)acrylate; a combination of a copolymer of branched (meth)acrylate and linear (meth)acrylate with at least one selected from homopolymers and copolymers of branched (meth)acrylate and at least one selected from homopolymers and copolymers of linear (meth)acrylate. From the viewpoint of improving cushioning properties, a combination of at least one selected from homopolymers and copolymers of branched (meth)acrylate and at least one selected from homopolymers and copolymers of linear (meth)acrylate is preferred, and a combination of at least one homopolymer of branched (meth)acrylate and at least one copolymer of linear (meth)acrylate is more preferred. In this case, the mass proportion of at least one selected from homopolymers and copolymers of branched (meth)acrylates in the poly(meth)acrylate (d) is the mass proportion of monomer units derived from the branched (meth)acrylate.

[0058] The branched (meth)acrylate is not particularly limited as long as it is a branched alkyl ester of (meth)acrylic acid, and a branched alkyl ester having 3 to 6 carbon atoms in the alkyl moiety is preferred, and a branched alkyl ester having 4 carbon atoms in the alkyl moiety is more preferred.

[0059] Examples of branched (meth)acrylates include alkyl acrylates such as isopropyl acrylate, t-butyl acrylate, sec-butyl acrylate, and isobutyl acrylate; and alkyl methacrylates such as isopropyl methacrylate, t-butyl methacrylate, sec-butyl methacrylate, and isobutyl methacrylate. Of these, isopropyl acrylate, isobutyl acrylate, isopropyl methacrylate, and isobutyl methacrylate are preferred.

[0060] Specific examples of the poly(meth)acrylate (d) include homopolymers of the above-mentioned branched (meth)acrylates, specifically poly(alkyl acrylates) such as poly(isopropyl acrylate), poly(t-butyl acrylate), poly(sec-butyl acrylate), poly(isobutyl acrylate), and poly(2-ethylhexyl acrylate); and poly(alkyl methacrylates) such as poly(isopropyl methacrylate), poly(t-butyl methacrylate), poly(sec-butyl methacrylate), poly(isobutyl methacrylate), and poly(2-ethylhexyl methacrylate). Of these, poly(isopropyl acrylate), poly(isobutyl acrylate), poly(isopropyl methacrylate), and poly(isobutyl methacrylate) are preferred.

[0061] Specific examples of the poly(meth)acrylate (d) include a combination of a homopolymer of the above-mentioned branched (meth)acrylate with a homopolymer of a linear (meth)acrylate or a copolymer of two or more linear (meth)acrylates, in which the content of the branched (meth)acrylate monomer unit in the poly(meth)acrylate (d) is 10% by mass or more.

[0062] As the linear (meth)acrylate, a linear alkyl ester having 1 to 10 carbon atoms in the alkyl portion is preferred, and a linear alkyl ester having 1 to 8 carbon atoms in the alkyl portion is more preferred.

[0063] Examples of linear (meth)acrylates include alkyl acrylates such as methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, n-pentyl acrylate, n-hexyl acrylate, n-heptyl acrylate, and n-octyl acrylate; and alkyl methacrylates such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, n-butyl methacrylate, n-pentyl methacrylate, n-hexyl methacrylate, n-heptyl methacrylate, and n-octyl methacrylate. Of these, methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, n-butyl methacrylate, n-pentyl methacrylate, n-hexyl methacrylate, and n-heptyl methacrylate are preferred.

[0064] Examples of homopolymers of linear poly(meth)acrylates include poly(alkyl acrylates) such as poly(methyl acrylate), poly(ethyl acrylate), poly(n-propyl acrylate), poly(n-butyl acrylate), poly(n-pentyl acrylate), poly(n-hexyl acrylate), poly(n-heptyl acrylate), and poly(n-octyl acrylate); and poly(alkyl methacrylates) such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, n-butyl methacrylate, n-pentyl methacrylate, n-hexyl methacrylate, n-heptyl methacrylate, and n-octyl methacrylate. Of these, poly(methyl acrylate), poly(ethyl acrylate), poly(n-propyl acrylate), poly(n-butyl acrylate), poly(methyl methacrylate), poly(ethyl methacrylate), poly(n-propyl methacrylate), poly(n-butyl methacrylate), poly(n-pentyl methacrylate), poly(n-hexyl methacrylate), poly(n-heptyl methacrylate), and the like are preferred.

[0065] Examples of copolymers of linear poly(meth)acrylates include copolymers of two or more of the above linear (meth)acrylates. Specific examples include copolymers of two or more selected from methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, n-butyl methacrylate, n-pentyl methacrylate, n-hexyl methacrylate, and n-heptyl methacrylate. Of these, copolymers of two or more selected from methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, and n-butyl methacrylate are preferred.

[0066] The content of poly(meth)acrylate (d) in the foamable vinyl chloride resin composition (B) is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, and even more preferably 0.10 parts by mass or more, and is preferably 5.0 parts by mass or less, and more preferably 4.0 parts by mass or less, relative to 100 parts by mass of the vinyl chloride resin. When the content of poly(meth)acrylate (d) is within the above-mentioned range, the cell diameter of the foam cells (air bubbles) in the foamed vinyl chloride resin molded sheet (Y) can be made finer, resulting in a surface with excellent cushioning properties.

[0067] [Plasticizer (e)] The expandable vinyl chloride resin composition (B) preferably further contains a plasticizer. If the expandable vinyl chloride resin composition (B) further contains a plasticizer, the flexibility of the foamed vinyl chloride resin molded sheet (Y) can be improved, and the cushioning properties can be further enhanced.

[0068] The type of plasticizer (e) that can be contained in the foamable vinyl chloride resin composition (B) can be appropriately selected from the range of types of plasticizers in the vinyl chloride resin composition (A) described above in the section "Vinyl chloride resin molded sheet (X)." From the viewpoint of further improving the cushioning properties of the surface, it is preferable to use at least a primary plasticizer as the plasticizer (e), and it is more preferable to use a primary plasticizer and a secondary plasticizer in combination. Specifically, it is preferable to use a trimellitic acid ester and / or a pyromellitic acid ester as the plasticizer (e), it is more preferable to use at least a trimellitic acid ester, and it is even more preferable to use a trimellitic acid ester in combination with epoxidized soybean oil.

[0069] The content of the trimellitic acid ester in the foamable vinyl chloride resin composition (B) is preferably 50 parts by mass or more, more preferably 70 parts by mass or more, and even more preferably 80 parts by mass or more, relative to 100 parts by mass of the vinyl chloride resin. It is also preferably 195 parts by mass or less, more preferably 145 parts by mass or less, even more preferably 125 parts by mass or less, and even more preferably 95 parts by mass or less. When the content of the trimellitic acid ester in the foamable vinyl chloride resin composition (B) is equal to or greater than the above-mentioned lower limit, the flexibility of the foamed vinyl chloride resin molded sheet (Y) can be further improved, and the cushioning properties of the surface layer can be further enhanced. On the other hand, when the content of the trimellitic acid ester in the foamable vinyl chloride resin composition (B) is equal to or less than the above-mentioned upper limit, the flexibility of the foamed vinyl chloride resin molded sheet (Y) can be prevented from becoming excessively high, and the strength of the foam cells (air bubbles) can be increased. This allows the surface layer having the foamed vinyl chloride resin molded sheet (Y) to maintain good cushioning properties.

[0070] The content of epoxidized soybean oil in the expandable vinyl chloride resin composition (B) is not particularly limited, but can be, for example, from 0 to 8 parts by mass, preferably 1 part by mass or more, and preferably 5 parts by mass or less, per 100 parts by mass of vinyl chloride resin.

[0071] The total content of plasticizers in the expandable vinyl chloride resin composition (B) (i.e., the content of plasticizer (e)) is preferably 50 parts by mass or more, more preferably 70 parts by mass or more, and even more preferably 80 parts by mass or more, relative to 100 parts by mass of vinyl chloride resin. It is also preferably 200 parts by mass or less, more preferably 150 parts by mass or less, and even more preferably 130 parts by mass or less. When the content of plasticizer (e) in the expandable vinyl chloride resin composition (B) is equal to or greater than the above-mentioned lower limit, the flexibility of the foamed vinyl chloride resin molded sheet (Y) can be further improved, and the cushioning properties of the surface layer can be further enhanced. On the other hand, when the content of plasticizer (e) in the expandable vinyl chloride resin composition (B) is equal to or less than the above-mentioned upper limit, the flexibility of the foamed vinyl chloride resin molded sheet (Y) can be prevented from becoming excessively high, and the strength of the foam cells (air bubbles) can be increased. This allows the surface layer having the foamed vinyl chloride resin molded sheet (Y) to maintain good cushioning properties.

[0072] [Additives] The expandable vinyl chloride resin composition (B) may further contain various additives other than the components described above. The various additives that may be contained in the expandable vinyl chloride resin composition (B) include the additives that may be contained in the vinyl chloride resin composition (A) described above in the section "Vinyl chloride resin molded sheet (X)." The content of the various additives in the expandable vinyl chloride resin composition (B) can be adjusted as appropriate within a range that achieves the desired effects of the present invention.

[0073] [Other Polymers] The foamable vinyl chloride resin composition (B) may further contain other polymers besides poly(meth)acrylate, as long as the effects of the present invention are not impaired. For example, a copolymer of (meth)acrylate and other monomers may be used. Examples of other monomers include ethylenically unsaturated carboxylic acid monomers and α,β-unsaturated nitrile monomers.

[0074] As the ethylenically unsaturated carboxylic acid monomer, at least one of an ethylenically unsaturated carboxylic acid and a salt thereof can be used. Examples of the ethylenically unsaturated carboxylic acid include an ethylenically unsaturated monocarboxylic acid and a derivative thereof, an ethylenically unsaturated dicarboxylic acid and an anhydride thereof, and a derivative thereof. Examples of the ethylenically unsaturated carboxylic acid salt include a sodium salt, a potassium salt, and a lithium salt of an ethylenically unsaturated carboxylic acid. One type of ethylenically unsaturated carboxylic acid and a salt thereof may be used alone, or two or more types may be used in combination in any ratio.

[0075] Examples of ethylenically unsaturated monocarboxylic acids include acrylic acid, methacrylic acid, and crotonic acid. Examples of derivatives of ethylenically unsaturated monocarboxylic acids include 2-ethylacrylic acid, isocrotonic acid, α-acetoxyacrylic acid, β-trans-aryloxyacrylic acid, α-chloro-β-E-methoxyacrylic acid, and β-diaminoacrylic acid. Examples of ethylenically unsaturated dicarboxylic acids include maleic acid, fumaric acid, and itaconic acid. Examples of acid anhydrides of ethylenically unsaturated dicarboxylic acids include maleic anhydride, diacrylic anhydride, methylmaleic anhydride, and dimethylmaleic anhydride. Examples of derivatives of ethylenically unsaturated dicarboxylic acids include methylmaleic acid, dimethylmaleic acid, phenylmaleic acid, chloromaleic acid, dichloromaleic acid, and fluoromaleic acid.

[0076] Examples of the α,β-unsaturated nitrile monomer include acrylonitrile and methacrylonitrile, which may be used singly or in combination of two or more.

[0077] [Method for Preparing Expandable Vinyl Chloride Resin Composition (B)] The expandable vinyl chloride resin composition (B) can be prepared by mixing the above-mentioned components without any particular limitation. The method for mixing the vinyl chloride resin, blowing agent, poly(meth)acrylate (d), optional plasticizer (e), other additives, and other polymers is not particularly limited. For example, components other than the dusting agent containing vinyl chloride resin microparticles and the blowing agent are mixed by dry blending, and then the dusting agent and the blowing agent are added and mixed. A Henschel mixer is preferably used for dry blending. The temperature during dry blending is not particularly limited, but is preferably 50°C or higher, more preferably 70°C or higher, and preferably 200°C or lower. The temperature during addition of the blowing agent can be set arbitrarily within a range that achieves the desired effects of the present invention, depending on the type of blowing agent used.

[0078] (Method for manufacturing a surface skin) The method for manufacturing a surface skin of the present invention is a method for manufacturing a surface skin having a vinyl chloride resin molded sheet (X) and a foamed vinyl chloride resin molded sheet (Y), and is characterized by comprising: a first step of forming the vinyl chloride resin molded sheet (X) using a vinyl chloride resin composition (A) containing a vinyl chloride resin and a predetermined amount of a plasticizer; and a second step of forming the foamed vinyl chloride resin molded sheet (Y) on one side in the thickness direction of the vinyl chloride resin molded sheet (X) using an expandable vinyl chloride resin composition (B). According to the method for manufacturing a surface skin of the present invention, a surface skin with excellent cushioning properties can be manufactured.

[0079] <First Step> In the first step, a vinyl chloride resin molded sheet (X) is formed using a vinyl chloride resin composition (A) containing a vinyl chloride resin and a predetermined amount of a plasticizer. Typically, the vinyl chloride resin composition (A) is molded into a sheet by a known molding method to form the vinyl chloride resin molded sheet (X). Here, the vinyl chloride resin composition (A) used to form the vinyl chloride resin molded sheet (X) described above in the "Skin" section can be used as the vinyl chloride resin composition (A). Furthermore, powder molding is preferably used as the molding method, and powder slush molding is more preferably used.

[0080] The mold temperature during powder slush molding is not particularly limited, but is preferably 200°C or higher, more preferably 220°C or higher, and is preferably 300°C or lower, more preferably 280°C or lower.

[0081] The vinyl chloride resin molded sheet (X) can be produced by any method, including, but not limited to, the following method. Specifically, the vinyl chloride resin composition (A) is sprinkled onto a mold at the temperature range described above, and the mold is left standing for 5 to 30 seconds. The excess vinyl chloride resin composition (A) is then shaken off, and the mold is then left standing at any temperature for 30 seconds to 3 minutes. The resulting vinyl chloride resin molded sheet (X) may or may not be released from the mold by cooling the mold to 10 to 60°C, depending on the aspect of the second step described below. The released vinyl chloride resin molded sheet is obtained, for example, as a sheet-like molded product conforming to the shape of the mold.

[0082] <Second Step> In the second step, a foamed vinyl chloride resin molded sheet (Y) is formed on one side in the thickness direction of the vinyl chloride resin molded sheet (X) using the foamable vinyl chloride resin composition (B). As the foamable vinyl chloride resin composition (B), the foamable vinyl chloride resin composition (B) used to form the foamed vinyl chloride resin molded sheet (Y) described above in the section "Skin" can be used. The method for forming a foamed vinyl chloride resin molded sheet (Y) using the expandable vinyl chloride resin composition (B) on one side in the thickness direction of the vinyl chloride resin molded sheet (X) is not particularly limited, and a method may be employed in which the expandable vinyl chloride resin composition (B) is foamed and molded into a sheet by the known molding method described above in the section "First Step" to produce a single foamed vinyl chloride resin molded sheet (Y), and then the foamed vinyl chloride resin molded sheet (Y) is bonded to one side in the thickness direction of the vinyl chloride resin molded sheet (X) by a known bonding method. However, the following method (sometimes referred to as "double slush molding") may also be used in which powder slush molding as a first step and powder slush molding as a second step are carried out consecutively using the same mold. That is, in the powder slush molding as the first step described above, excess vinyl chloride resin composition (A) is shaken off from the mold, and the resulting vinyl chloride resin molded sheet (X) is left standing at an arbitrary temperature for 30 seconds to 3 minutes without being demolded from the mold. Instead, in the second step, a powder of the expandable vinyl chloride resin composition (B) is sprinkled onto the mold with the vinyl chloride resin molded sheet (X) attached to it to foam it. The mold temperature when the powder of the expandable vinyl chloride resin composition (B) is sprinkled is not particularly limited, but is preferably 200°C or higher, more preferably 220°C or higher, and preferably 300°C or lower, and more preferably 280°C or lower. After leaving the mold for 5 seconds to 30 seconds, excess expandable vinyl chloride resin composition (B) is shaken off, and the resulting mold is left standing at an arbitrary temperature for 30 seconds to 3 minutes. The mold is then cooled to 10°C to 60°C, and the resulting skin is demolded from the mold.The demolded skin has a foamed vinyl chloride resin molded sheet (Y) disposed on one side in the thickness direction of the vinyl chloride resin molded sheet (X), and in one example of the above-mentioned production method, the obtained skin is a sheet-like molded article with a two-layer structure that generally follows the shape of the mold. Thus, by carrying out powder slush molding twice in succession using the same mold as the first and second steps in the skin production method of the present invention, it is possible to efficiently produce a skin having a foamed vinyl chloride resin molded sheet (Y) disposed on one side in the thickness direction of the vinyl chloride resin molded sheet (X).

[0083] The above description has been given of the case where the method for producing a skin of the present invention produces a skin in which a foamed vinyl chloride resin molded sheet (Y) is directly bonded to one surface in the thickness direction of a molded vinyl chloride resin sheet (X), but the method for producing a skin of the present invention is not limited to this. For example, the method for producing a skin of the present invention can also produce a skin in which a molded vinyl chloride resin sheet (X) and a foamed vinyl chloride resin molded sheet (Y) are bonded together via another resin layer or the like by including any step other than the above-mentioned first and second steps.

[0084] (Laminate) The laminate of the present invention comprises a foamed polyurethane molded product and the above-described surface skin of the present invention. The laminate of the present invention has a structure in which the above-described foamed vinyl chloride resin molded sheet (Y) is disposed between the foamed polyurethane molded product and the above-described foamed vinyl chloride resin molded sheet (X). The laminate of the present invention has excellent cushioning properties due to the presence of the above-described surface skin of the present invention.

[0085] Typically, the polyurethane foam is backed by the foamed vinyl chloride resin sheet (Y) on the skin side, and the polyurethane foam and the skin are adjacent to each other in the lamination direction (i.e., the polyurethane foam and the vinyl chloride resin sheet (X) are laminated in the lamination direction via the foamed vinyl chloride resin sheet (Y)). The laminate of the present invention effectively suppresses thermal shrinkage because the foamed vinyl chloride resin sheet (Y) is interposed between the polyurethane foam and the vinyl chloride resin sheet (X). Therefore, the laminate of the present invention is suitable for use as an automobile interior material for automobile interior parts such as automobile instrument panels and door trims, and is particularly suitable for use in automobile instrument panels.

[0086] The lamination method is not particularly limited, and the following method can be used, for example: isocyanates and polyols, which are raw materials for the foamed polyurethane molded body, are reacted and polymerized on the surface of the surface on which the foamed vinyl chloride resin molded sheet (Y) is placed, and polyurethane is foamed by a known method, thereby forming a foamed polyurethane molded body directly on the surface.

[0087] The present invention will be specifically described below based on examples, but the present invention is not limited to these examples. In the following description, "%" and "parts" representing amounts are based on mass unless otherwise specified.

[0088] The skins of the examples and comparative examples were evaluated as follows.

[0089] <Density, Magnification, and Thickness> For the skins of the Examples and Comparative Examples, a molded article of the surface layer resin composition (vinyl chloride resin composition (A)) and a molded article of the foam layer resin composition (a composition obtained by removing the foaming agent from the expandable vinyl chloride resin composition (B)) were prepared in advance, and the density of each was measured using the underwater displacement method of JIS K7112-1. The molding conditions (heating temperature and time) for the molded articles were the same as those for the corresponding Examples and Comparative Examples. The skins of the Examples were cut into specimens measuring 50 mm x 50 mm. After measuring the weight of the specimens, the cross sections were examined using an optical microscope (model: Digital Microscope VHX-6000, manufactured by Keyence Corporation) to measure the thicknesses of the skin, surface layer (molded vinyl chloride resin sheet (X)), and foam layer (molded foam vinyl chloride resin sheet (Y)). The weight of the foam layer was determined by subtracting the weight of the surface layer from the weight of the test specimen. The volume of the foam layer was also determined from the cross-sectional thickness. The density was determined by dividing the weight of the foam layer by the volume of the foam layer. The magnification was determined by dividing the foam layer density by the density of a molded article (molded article without foaming agent) made from the foam layer resin composition excluding the corresponding foaming agent. Density of foam layer (foamed vinyl chloride resin molded sheet (Y)) = (test piece (skin weight) - surface layer weight) ÷ foam layer volume Magnification of foam layer (foamed vinyl chloride resin molded sheet (Y)) = foam layer density ÷ density of molded article without foaming agent

[0090] <Cushioning properties> Test specimens were prepared by cutting the skins of the Examples and Comparative Examples to dimensions of 50 mm x 50 mm. Under an environment of 23°C temperature and 50% RH, a probe was pressed from the side of the molded vinyl chloride resin sheet (X) using a Rhesca "TAC-1000" with a probe diameter of 10 mm and a pressing speed of 0.1 mm / s, and the amount of indentation displacement of the test specimen when a pressing load reached 1200 gf was measured. Note that a larger amount of indentation displacement indicates a more excellent cushioning property of the skin.

[0091] <Average Values ​​of Void Ratio and Foam Cell Volume> For the skins of the Examples and Comparative Examples, the vinyl chloride resin sheet (X) and the foamed vinyl chloride resin molded sheet (Y) were measured (measurement area 8 mm x 8 mm) using a multi-three-dimensional measurement X-ray CT device (manufactured by Yamato Scientific Co., Ltd.), and the obtained CT data was reconstructed into 3D data, which was then analyzed using the "Foam / Powder Analysis Module" function of the industrial CT software "VG Studio MAX" by System Create Co., Ltd. The analysis was performed on the foamed vinyl chloride resin molded sheet (Y) only, and the volume of the foam cells and the volume of the parts other than the foam cells were measured. The average value and standard deviation were determined from the measured values ​​of the foam cell volume. The void ratio was also calculated using the following formula: Void ratio (%) = 100 x {volume of foam cells ÷ (volume of parts other than foam cells + volume of foam cells)}

[0092] Example 1 Preparation of Vinyl Chloride Resin Composition (A) Of the ingredients shown for vinyl chloride resin composition (A) in Table 1, all ingredients except for the plasticizer and the vinyl chloride resin fine particles serving as a dusting agent were placed in a Henschel mixer and mixed. When the temperature of the mixture rose to 80°C, all of the plasticizer was added, and the mixture was further heated to dry up (a state in which the plasticizer is absorbed into the vinyl chloride resin particles serving as the vinyl chloride resin, and the mixture becomes smooth). When the dried-up mixture was cooled to a temperature of 100°C or below, the vinyl chloride resin fine particles serving as a dusting agent were added, thereby preparing vinyl chloride resin composition (A).

[0093] Preparation of Expandable Vinyl Chloride Resin Composition (B) Of the ingredients shown in Example 1 in Table 1, all but the plasticizer, the vinyl chloride resin fine particles serving as a dusting agent, and the thermally decomposable blowing agent were placed in a Henschel mixer and mixed. When the temperature of the mixture rose to 80°C, all of the plasticizer was added, and the mixture was further heated to dry up (a state in which the plasticizer is absorbed into the vinyl chloride resin particles serving as the vinyl chloride resin, resulting in a smooth mixture). When the dried-up mixture was cooled to a temperature of 100°C or below, the vinyl chloride resin fine particles serving as a dusting agent were added, and when the temperature further dropped to 80°C, the thermally decomposable blowing agent was added, thereby preparing the expandable vinyl chloride resin composition (B).

[0094] <Preparation of Skin> [Step 1 (Formation of Vinyl Chloride Resin Molded Sheet (X))] The vinyl chloride resin composition (A) obtained above was sprinkled onto a textured mold heated to a temperature of 260°C, and left to melt for any time period of about 8 to 20 seconds, after which excess vinyl chloride resin composition (A) was shaken off.

[0095] [Step 2 (Formation of Foamed Vinyl Chloride Resin Sheet (Y))] Following Step 1, the foamable vinyl chloride resin composition (B) obtained above was further sprinkled onto the vinyl chloride resin molded sheet (X) attached to the textured mold. The sheet was left to melt and foam for a period of approximately 10 to 30 seconds, after which excess foamable vinyl chloride resin composition (B) was shaken off. The textured mold was then placed in an oven set at 220°C, and after 60 seconds of standing, the textured mold was cooled with cooling water. Once the mold temperature had cooled to 40°C, a skin measuring 200 mm in length and 300 mm in width was removed from the mold. The resulting skin was a two-layer sheet in which the foamed vinyl chloride resin molded sheet (Y) was laminated on one side of the vinyl chloride resin molded sheet (X) in the thickness direction. The resulting skin was evaluated for the above-mentioned properties. The results are shown in Table 1.

[0096] (Examples 2 to 7, Comparative Examples 1 and 2) For examples and comparative examples other than Example 1, skins were prepared and the properties were evaluated in the same manner as in Example 1. Table 1 shows the results.

[0097]

[0098] 1) Shin-Dai-Ichi Vinyl Corporation, product name "ZEST (registered trademark) 1700ZI" (suspension polymerization method, average degree of polymerization: 1700, average particle size: 130 μm) 2) Shin-Dai-Ichi Vinyl Corporation, product name "ZEST PQLTX" (prepared by emulsion polymerization method, average degree of polymerization: 800, average particle size: 1.8 μm) 3) Mitsubishi Gas Chemical Company, product name "TOTM", tri-2-ethylhexyl trimellitate 4) ADEKA Corporation, product name "ADEKACIZER O-130S" 5) Kyowa Chemical Industry Co., Ltd., product name "ALCAMIZER (registered trademark) 5" 6) Mizusawa Industrial Chemicals, product name "MIZUKALIZER DS" 7) Showa Denko K.K., product name "Karenz DK-1" 8) Sakai Chemical Industry Co., Ltd., product name "SAKAI SZ2000" 9) ADEKA Corporation, product name "ADEKA STAB LS-12" 10) Linear poly(meth)acrylate synthesized as follows: 300 parts of ion-exchanged water, 50 parts of methyl methacrylate (MMA), 20 parts of n-butyl acrylate (BA), 30 parts of n-butyl methacrylate (BMA), 1 part of n-octyl mercaptan, and 1.1 parts of sodium dodecylbenzenesulfonate were charged into a reaction vessel equipped with a stirrer and reflux condenser. After nitrogen substitution with stirring, the internal temperature was raised to 60°C, and 0.15 parts of potassium persulfate and 5 parts of ion-exchanged water were added. Heating and stirring were continued for 2 hours to terminate the polymerization, yielding a latex-like reaction product. The resulting latex-like reaction product was cooled and then spray-dried at an inlet temperature of 150°C and an outlet temperature of 65°C to yield a polymer. The obtained polymer was measured by GPC to find that the number average molecular weight (Mn) was 50,000 and the weight average molecular weight (Mw) was 220,000. The composition ratio (mass ratio) was determined by NMR to find that MMA:BA:BMA = 49:22:29. Mn and Mw are values ​​calculated in terms of polystyrene by gel permeation chromatography (GPC) using tetrahydrofuran (THF) as a solvent. The composition ratio (mass ratio) by NMR was found to be 1The values ​​were calculated from the proton integral ratio of H-NMR. 11) Product name "TCI" (poly(isobutyl methacrylate) manufactured by Tokyo Chemical Industry Co., Ltd. Mn 30,000, Mw 52,000 by GPC (conditions as above). 12) Product name "UNIFOAM AZ P-4" manufactured by Otsuka Chemical Co., Ltd. 13) Product name "DA PX 1720(A) Black" manufactured by Dainichiseika Color & Chemicals Co., Ltd. 14) Product name "DA P 1050 White" manufactured by Dainichiseika Color & Chemicals Co., Ltd.

[0099] A comparison of Comparative Example 1 and Example 1 in Table 1 shows that the use of a poly(meth)acrylate containing a predetermined amount of branched (meth)acrylate monomer units in the foamed vinyl chloride resin molded sheet (Y) results in finer foam cells and superior cushioning properties for the surface. A comparison of Comparative Example 2 and Example 1 shows that the inclusion of branched (meth)acrylate monomer units in the poly(meth)acrylate is effective in finer foam cells and improving the cushioning properties of the surface. Examples 2 to 4 are examples in which the amount of branched poly(meth)acrylate was varied, but similar to Example 1, finer foam cells and improved cushioning properties for the surface were confirmed. Furthermore, Examples 5 and 6 are examples in which a branched poly(meth)acrylate and a linear poly(meth)acrylate were used in combination. The poly(meth)acrylate contains branched (meth)acrylate monomer units and linear (meth)acrylate monomer units, and it was found that the combination provided excellent cushioning properties. As shown in Example 7, even when the amount of foaming agent is changed, the effects of the present invention of making the foam cells finer and improving the cushioning properties of the surface can be obtained.

[0100] According to the present invention, it is possible to provide a surface skin having excellent cushioning properties. Furthermore, according to the present invention, it is possible to provide a laminate having the surface skin and having excellent cushioning properties.

Claims

1. A skin having a vinyl chloride resin molded sheet (X) and a foamed vinyl chloride resin molded sheet (Y) arranged on one side of the vinyl chloride resin molded sheet (X) in the thickness direction, wherein the vinyl chloride resin molded sheet (X) contains a vinyl chloride resin (a) and a plasticizer (b), the content of the plasticizer (b) in the vinyl chloride resin molded sheet (X) is 50 parts by mass or more per 100 parts by mass of the vinyl chloride resin (a), the foamed vinyl chloride resin molded sheet (Y) contains a vinyl chloride resin (c) and a poly(meth)acrylate (d), and the poly(meth)acrylate (d) contains 10% by mass or more of monomer units derived from a branched alkyl ester (meth)acrylate.

2. The skin according to claim 1, wherein the poly(meth)acrylate (c) is at least one selected from homopolymers and copolymers of (meth)acrylates which are branched alkyl esters, or a combination of at least one selected from homopolymers and copolymers of (meth)acrylates which are branched alkyl esters and at least one selected from homopolymers and copolymers of (meth)acrylates which are linear alkyl esters.

3. The skin according to claim 1, wherein the content of the poly(meth)acrylate (d) in the foamed polyvinyl chloride resin molded sheet (Y) is 0.01 parts by mass or more and 5.0 parts by mass or less per 100 parts by mass of the polyvinyl chloride resin (c).

4. The skin according to claim 1, wherein the foamed polyvinyl chloride resin molded sheet (Y) further contains a plasticizer (e), and the content of the plasticizer (e) in the foamed polyvinyl chloride resin molded sheet (Y) is 50 parts by mass or more and 200 parts by mass or less per 100 parts by mass of the polyvinyl chloride resin (c).

5. The skin according to claim 1, wherein the foamed polyvinyl chloride resin molded sheet (Y) further contains an azo compound, and the content of the azo compound in the foamed polyvinyl chloride resin molded sheet (Y) is 0.05 parts by mass or more and 1.00 parts by mass or less per 100 parts by mass of the polyvinyl chloride resin (c).

6. The skin according to claim 1, wherein the foamed polyvinyl chloride resin molded sheet (Y) has a thickness of 1.5 mm or more.

7. The skin according to any one of claims 1 to 6, which is used as a skin for an automobile interior part.

8. A method for producing a skin having a vinyl chloride resin molded sheet (X) and a foamed vinyl chloride resin molded sheet (Y), comprising: a first step of forming a vinyl chloride resin molded sheet (X) using a vinyl chloride resin composition (A) containing a vinyl chloride resin (a) and a plasticizer (b); and a second step of forming a foamed vinyl chloride resin molded sheet (Y) using an expandable vinyl chloride resin composition (B) on one side in the thickness direction of the vinyl chloride resin molded sheet (X), wherein the content of the plasticizer (b) in the vinyl chloride resin composition (A) is 50 parts by mass or more per 100 parts by mass of the vinyl chloride resin (a), the foamed vinyl chloride resin molded sheet (Y) contains vinyl chloride resin (c) and a poly(meth)acrylate (d), and the poly(meth)acrylate (d) contains 10% by mass or more of a monomer unit derived from a branched alkyl ester (meth)acrylate.

9. A laminate comprising a polyurethane foam and a skin according to any one of claims 1 to 6, wherein the polyvinyl chloride resin foamed sheet (Y) is disposed between the polyurethane foam and the polyvinyl chloride resin foamed sheet (X).

Citation Information

Patent Citations

  • Vinyl chloride resin composition for foam sheet

    JP1996120109A

  • Foaming cell conditioner for vinyl chloride resin, vinyl chloride resin composition containing the same and foam molding

    JP2021054947A

  • Processing assistant for expansion molding, vinyl chloride resin composition for expansion molding, and expansion molded body

    WO2010061630A1

  • Skin, method for producing skin, and layered product

    WO2019188520A1