Fullerene derivative, method for synthesizing fullerene derivative, method for producing fullerene derivative, vapor-deposited product, and method for producing vapor-deposited product

The synthesis of tert-butyl indanoflerenone using arylfullerene dimer oxidation in hydrohalic acid addresses the challenge of forming amorphous fullerene derivative films, ensuring stable integration into devices with improved sublimation temperature and cost-effectiveness.

WO2024203608A1PCT designated stage expired Publication Date: 2024-10-03MITSUBISHI CORPORATION
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010724
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-12-05
Filing Date
2024-03-19
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing fullerene derivatives struggle to form vapor-deposited films with an amorphous structure, which is essential for implementing them in devices like photoelectric conversion elements and image sensors due to their high light absorption and electrical properties.

Method used

A fullerene derivative with a specific formula, such as tert-butyl indanoflerenone, is synthesized using an arylfullerene dimer oxidation process in the presence of hydrohalic acid, resulting in a film that maintains an amorphous structure even after annealing or exposure to solvent vapor, preventing crystallization and device defects.

Benefits of technology

The fullerene derivative achieves a stable amorphous structure for a long period, lowers the sublimation temperature, and enables efficient integration into various devices, reducing manufacturing costs and ensuring uniform film formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010724_03102024_PF_FP_ABST
    Figure JP2024010724_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This fullerene derivative is represented by formula (1) (wherein FLN represents a fullerene framework; X represents a halogen group or an organic group; and Y represents O or S).
Need to check novelty before this filing date? Find Prior Art

Description

Fullerene derivative, synthesis reaction of fullerene derivative, method for producing fullerene derivative, deposition product, and method for producing deposition product

[0001] The present invention relates to a fullerene derivative, a synthesis reaction of a fullerene derivative, a method for producing a fullerene derivative, a deposition product, and a method for producing a deposition product.

[0002] In the development of devices such as photoelectric conversion elements or image sensors, attention has been focused on technologies using vapor-depositable fullerenes or derivatives thereof that have high light absorption properties and good electrical properties. As such fullerene derivatives, Patent Document 1 discloses a fullerene having a structure in which indanone is condensed with fullerene.

[0003] International Publication No. 2021 / 149801

[0004] Although there are several fullerene derivatives that can be vapor-deposited, the vapor-deposited films containing the fullerene derivatives do not have an amorphous structure, making them difficult to implement in various devices.

[0005] An object of the present invention is to provide a fullerene derivative which forms an amorphous structure in a vapor-deposited film.

[0006] The fullerene derivative of the present disclosure is represented by the formula (1):

[0007] (wherein FLN is a fullerene skeleton, X is a halogen group or an organic group, and Y is O or S).

[0008] According to one aspect of the present invention, a fullerene derivative can be provided that forms a vapor-deposited film with an amorphous structure.

[0009] FIG. 1 is a diagram showing the structural formula of tertiary butyl indanofullerene ketone (tBu-FIDO). FIG. 2 is a diagram showing the synthetic route of tBu-FIDO. FIG. 3 is a diagram showing the synthetic route of tBu-FIDO (synthetic route from dimer to ketone). FIG. 4 is a 1H NMR chart of 2-ethoxy-5-tertiary butylphenyl hydrogenated fullerene (intermediate). FIG. 5 is an enlarged view of a portion of the chart in FIG. 4. FIG. 6 is a 13C NMR chart of 2-ethoxy-5-tertiary butylphenyl hydrogenated fullerene (intermediate). FIG. 7 is an enlarged view of a portion of the chart in FIG. 6. FIG. 8 is a 13C NMR chart of tBu-FIDO. 60 1 is a graph showing the reduction potential of fullerenes and fullerene derivatives. 2 is a table showing the reduction potential and electron affinity of fullerenes and fullerene derivatives. 60 ) is a diagram showing the structural formula of indanofullerene ketone (H-FIDO). FIG. 1 is a diagram showing the structural formula of methoxyindanofullerene ketone (MeO-FIDO). FIG. 2 is a diagram showing the structural formula of fluoroindanofullerene ketone (F-FIDO). FIG. 3 is a diagram showing the structural formula of methylindanofullerene ketone (Me-FIDO). C 60 Graph showing X-ray diffraction patterns of H-FIDO immediately after deposition, before and after annealing. Graph showing X-ray diffraction patterns of H-FIDO immediately after deposition, before and after annealing. Graph showing X-ray diffraction patterns of Me-FIDO immediately after deposition, before and after annealing. Graph showing X-ray diffraction patterns of tBu-FIDO immediately after deposition, before and after annealing. Graph showing X-ray diffraction patterns of tBu-FIDO immediately after deposition, before and after annealing. Graph showing transmission electron microscope (TEM) images (left and upper right) and X-ray diffraction image (lower right) of tBu-FIDO. Graph showing TEM images (left and upper right) and X-ray diffraction image (lower right) of H-FIDO after annealing. Graph showing TEM images (left and upper right) and X-ray diffraction image (lower right) of H-FIDO after annealing. 60 1 is a graph showing a thermogravimetric analysis (TGA) chart of [6,6]-phenyl-C 61 -Butyric acid methyl ester (PC 611 is a graph showing a TGA chart of a fullerene derivative (BM). 2 is a graph showing a TGA chart of H-FIDO. 3 is a graph showing a TGA chart of Me-FIDO. 4 is a graph showing a TGA chart of tBu-FIDO. 5 is a table showing TGA results of fullerene derivatives. 6 is a table showing currents during sublimation of fullerene derivatives. 7 is a graph showing X-ray diffraction charts of fullerene and tBu-FIDO. 8 is a graph showing X-ray diffraction charts of a tBu-FIDO thin film one month after deposition, one month after annealing after deposition, and one month after exposure to solvent vapor after deposition. 9 is a graph showing X-ray diffraction charts of a fullerene thin film one day after deposition, one day after annealing after deposition, one day after exposure to solvent vapor after deposition, one month after deposition, one month after annealing after deposition, and one month after exposure to solvent vapor after deposition. 1 is a graph showing the relationship between wavelength and absorbance in ultraviolet-visible spectroscopy (UV-vis) of fullerene and tBu-FIDO. 2 is a table showing the results of vacuum thermogravimetry (vacuum TG) of fullerene derivatives. 3 is a diagram showing the structural formula of tertiary butyl indanoflurane thioketone (tBu-FIDS). 4 is a diagram showing the synthetic route of tBu-FIDS (reaction route from tBu-FIDO to tBu-FIDS). 5 is a 1H NMR chart of tBu-FIDS. 6 is a 13C NMR chart of tBu-FIDS. 7 is a graph showing a differential thermal analysis (DTA) chart of tBu-FIDS. 8 is a diagram showing the differential thermal analysis (DTA) chart of tBu-FIDS. 9 is a diagram showing the differential thermal analysis (DTA) chart of tBu-FIDS. 10 is a diagram showing the differential thermal analysis (DTA) chart of tBu-FIDS. 11 is a diagram showing the differential thermal analysis (DTA) chart of tBu-FIDS. 60 1 is a table showing the results of thermogravimetry (TG) of tBu-FIDO and tBu-FIDO. 60 3 is a graph showing the reduction potentials of tBu-FIDS, tBu-FIDO, and tBu-FIDO. 60 1 is a table showing the reduction potentials and electron affinities of tBu-FIDO and tBu-FIDS. 60 1 is a graph showing simulated and measured electron affinities of tBu-FIDO and tBu-FIDS.

[0010] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.

[0011] <Fullerene Derivative> The fullerene derivative of the present disclosure is represented by the above formula (1).

[0012] FLN in the above formula (1) is a fullerene skeleton.

[0013] The fullerene skeleton may be, for example, C 60 Skeleton, C 70 Skeleton, C 76 Skeleton, C 78 Among them, C 60 The skeleton is preferable. 60 Since C can be easily obtained industrially with higher purity than other fullerenes, 60 The purity of the fullerene derivative derived from the compound can be increased.

[0014] As represented by the above formula (1), the fullerene derivative of the present disclosure has a fullerene skeleton containing indanone (C 9 H 8 O) is condensed into indanofullerene.

[0015] Furthermore, X in the above formula (1) is a halogen group or an organic group.

[0016] Examples of the halogen group include a chlorine atom, a bromine atom, an iodine atom, etc. Among these, the chlorine atom is preferred as the halogen group.

[0017] Examples of the organic group include alkyl groups, heteroalkyl groups, alkenyl groups, heteroalkenyl groups, alkynyl groups, heteroalkynyl groups, cycloalkyl groups, heterocycloalkyl groups, aryl groups, heteroaryl groups, alkoxy groups, carbonyl groups, and imino groups, as well as combinations of two or more of these. The organic group may be either linear or branched, except for cyclic groups. The organic group may also have a substituent.

[0018] The number of carbon atoms in the organic group is preferably from 1 to 10, more preferably from 2 to 8, and even more preferably from 3 to 6. Among these, the organic group is preferably an alkyl group or an alkoxy group, more preferably an alkyl group having from 1 to 10 carbon atoms, and even more preferably a branched alkyl group having from 3 to 6 carbon atoms. An example of a branched alkyl group having from 3 to 6 carbon atoms is a tertiary butyl group.

[0019] Y in formula (1) is oxygen (O) or sulfur (S). When Y is O, the fullerene derivative of formula (1) has an indanofullerene ketone structure. Indanofullerene ketone is sometimes called indanofullerenone. When Y is S, the fullerene derivative has an indanofullerene thioketone structure.

[0020] The fullerene derivative represented by the above formula (1) is preferably a fullerene derivative represented by the following formula (2): The fullerene derivative represented by the following formula (2) has an indanoflerene ketone structure.

[0021]

[0022] In formula (2), tBu is a tertiary butyl group. The bonding position of tBu is not particularly limited. For example, tBu may be bonded to any of the 1st to 4th positions of the indanone skeleton constituting the fullerene derivative represented by formula (2) above. The bonding position of tBu is controlled by the raw materials used or the synthesis conditions.

[0023] The fullerene derivative represented by the above formula (2) is preferably a fullerene derivative represented by the following formula (3).

[0024]

[0025] In the fullerene derivative represented by the above formula (3), tBu is bonded to the 2-position (β-position) of the indanone skeleton constituting the fullerene derivative represented by the above formula (2). This fullerene derivative represented by the above formula (2) corresponds to tertiary butyl indanoflerenone shown in Figure 1. In this specification, tertiary butyl indanoflerenone may be abbreviated as tBu-FIDO.

[0026] The fullerene derivative represented by the above formula (1) is preferably a fullerene derivative represented by the following formula (4): The fullerene derivative represented by the following formula (4) has an indanoflurane thioketone structure.

[0027] In formula (4), tBu is a tertiary butyl group. The bonding position of tBu is not particularly limited. For example, tBu may be bonded to any of the 1st to 4th positions of the indanone skeleton constituting the fullerene derivative represented by formula (4) above. The bonding position of tBu is controlled by the raw materials used or the synthesis conditions.

[0028] The fullerene derivative represented by the above formula (4) is preferably a fullerene derivative represented by the following formula (5).

[0029]

[0030] In the fullerene derivative represented by the above formula (5), tBu is bonded to the 2-position (β-position) of the indanone skeleton constituting the fullerene derivative represented by the above formula (4). The fullerene derivative represented by the above formula (2) is a tertiary butyl indanoflurane thioketone shown in Figure 38. In this specification, tertiary butyl indanoflurane thioketone may be abbreviated as tBu-FIDS.

[0031] As described above, the fullerene derivatives of the present disclosure are fullerene derivatives represented by the above formulas (1) to (5), and therefore vapor-deposited films containing the fullerene derivatives can have an amorphous structure. Therefore, the fullerene derivatives of the present disclosure are expected to be applicable to various devices.

[0032] As described above, the fullerene derivative of the present disclosure is a fullerene derivative represented by the above formula (2), so that a vapor-deposited film containing the fullerene derivative has an amorphous structure and can maintain the amorphous structure even after annealing or exposure to solvent vapor. Note that annealing is performed by applying heat to the deposited material to remove residual stress in the deposited material and prevent deformation of the deposited material. Annealing may be performed in solvent vapor.

[0033] That is, the fullerene derivative represented by the above formula (2) shows almost no crystallinity even when annealed or exposed to solvent vapor after deposition, and therefore, it is possible to prevent device defects caused by crystallization when fabricating the device.

[0034] Furthermore, since the fullerene derivative of the present disclosure is a fullerene derivative represented by the above formula (3), the amorphous structure of the vapor-deposited film containing the fullerene derivative can be maintained for a long period of time, even after annealing or exposure to solvent vapor.

[0035] As described above, the fullerene derivatives of the present disclosure are those in which the fullerene skeleton is C 60 Skeleton, C 70 Skeleton, C 76 skeleton, and C 78 By using at least one selected from the group consisting of a fullerene derivative and a fullerene skeleton, the amorphous structure of the vapor-deposited film containing the fullerene derivative can be maintained for a long period of time, while the sublimation temperature of the vapor-deposited film containing the fullerene skeleton can be lower than that of fullerene. Furthermore, the fullerene derivatives of the formulas (2) and (3) can maintain the amorphous structure for a long period of time even after annealing or exposure to solvent vapor, while the sublimation temperature of the vapor-deposited film containing the fullerene skeleton can be lower than that of fullerene.

[0036] <Synthetic Reaction and Production Method of Fullerene Derivative> The fullerene derivative of the present disclosure can be produced using the synthetic reaction of the fullerene derivative shown below.

[0037] The synthesis reaction of the fullerene derivative is, for example, a synthesis reaction of a fullerene derivative having an indanofullerenone structure (when Y is oxygen) among the fullerene derivatives of the above formula (1). This reaction is a synthesis reaction of a fullerene derivative represented by the following formula (6) in which an arylfullerene dimer is oxidized in the presence of hydrohalic acid.

[0038]

[0039] In formula (6), FLN is a fullerene skeleton, and X is hydrogen, a halogen group, or an organic group. When X is hydrogen, this indicates that the aryl group to which X is bonded in the fullerene derivative represented by formula (6) above does not have a substituent. In other words, the aryl group to which X is bonded in the fullerene derivative represented by formula (6) above may have an optional substituent.

[0040] Here, the arylfullerene dimer is a precursor of a fullerene derivative, which is synthesized by oxidizing, in the presence of a base, an arylhydrofullerene that is synthesized by reacting a Grignard reagent with a fullerene.

[0041] The hydrohalic acid is an aqueous solution of hydrogen halide. Examples of the hydrogen halide include hydrogen chloride and hydrogen bromide. Among these, hydrobromic acid, which is an aqueous solution of hydrogen bromide, is preferred from the viewpoint of improving the reproducibility and yield of the obtained fullerene derivative.

[0042] The concentration of the hydrohalic acid as an aqueous solution is preferably 35 to 60%, more preferably 40 to 55%, and even more preferably 45 to 50%. When the hydrohalic acid has a concentration of 35 to 60%, it is easy to handle and the reproducibility and yield of the obtained fullerene derivative can be further improved. In particular, when 45 to 50% hydrobromic acid is used as the hydrohalic acid, the reproducibility and yield of the obtained fullerene derivative can be further improved.

[0043] Here, the synthesis reaction of the fullerene derivative represented by the above formula (6) will be specifically described. Figures 2 and 3 are diagrams showing the synthesis route of tertiary butyl indanoflerenone (tBu-FIDO), which is an example of a fullerene derivative.

[0044] As shown in FIG. 2, first, 2-ethoxy-5-tert-butylphenyl hydrogenated fullerene (hereinafter referred to as 1f) is synthesized. In the synthesis of 1f, C 60 (500 mg, 0.7 mmol) was dissolved in ortho-dichlorobenzene (o-DCB) (50.0 mL) containing 1,3-dimethyl-2-imidazolidinone (DMI) (2.3 mL, 21 mmol), and the solution was degassed three times and then purged with nitrogen (N 2 Next, Grignard reagent (2.0 mL, 2.1 mmol) was added to the flask at room temperature. 2 Added under atmosphere.

[0045] The Grignard reagent was synthesized as follows: First, a solution of 2-bromo-4-(tert-butyl)-1-(methoxymethyl)benzene (2.1 mL, 10.0 mmol) in anhydrous tetrahydrofuran (THF) (10.0 mL) was added to a 200 mL N 2 A trace amount of iodine (I) was added as an initiator under the atmosphere. 2 The solution was slowly added dropwise to polished magnesium (Mg) powder (360.0 mg, 15 mmol) in a 1000 mL flask. After vigorously stirring for 1 hour, a Grignard solution was obtained. This Grignard solution was transferred by a Schlenk operation and stored in a Schlenk flask. 2 The concentration of the Grignard reagent was confirmed to be 1.04 mol / L by anhydrous titration under atmospheric pressure using a trace amount of 1,10-phenanthroline as an indicator and methanol as a titrant.

[0046] Next, the Grignard reagent was added and stirred at room temperature for 15 minutes, after which the dark green reaction mixture was treated with CH 3 The reaction was quenched by the addition of COOH (160 μL, 2.8 mmol). The dark green reaction mixture quickly turned brown, and the reaction mixture was concentrated by evaporating the solvent under vacuum. Then, carbon disulfide (CS) was used as the eluent. 2 ) was used to obtain 2-ethoxy-5-tert-butylphenyl hydrogenated fullerene (1f) (565.8 mg, 90%) as a brownish powder.

[0047] If was identified from its H NMR chart (see Figures 4 and 5) and C NMR chart (see Figures 6 and 7). The NMR analysis results are shown below.

[0048] 1H NMR (600MHz, CS 2 / CDCl 3 ) δ8.50 (d, J=2.0Hz, 1H), 7.75 (d, J=8.1Hz, 1H), 7.61 (dd, J=8.1Hz, 2.0H z, 1H), 6.95 (s, 1H), 4.49 (s, 1H), 5.52 (s, 1H), 3.68 (s, 3H), 1.30 (s, 9H).

[0049] 13C{ 1 H}NMR (125MHz, CS 2 / CDCl 3 , all 1C unless specified) 8.50, 8.50.

[0050] Next, an arylfullerene dimer (hereinafter sometimes referred to as Dimer (1g)) was synthesized as shown in Figure 2. First, a solution of t-BuOK (67.0 μL, 0.067 mmol, 1 M) in THF was added to a solution of 1f (50.0 mg, 0.056 mmol) in 3.0 mL of anhydrous o-DCB solution at room temperature. 2 After stirring under atmospheric pressure for 15 minutes, N-bromosuccinimide (NBS) (39.9 mg, 0.224 mmol) was added. 2 The mixture was stirred vigorously at room temperature under atmospheric pressure for 12 hours. The resulting brownish suspension was then diluted with 0.5 mL of H 2 The mixture was quenched with 0 C and excess MeOH was added to precipitate the crude product. Finally, Dimer (1 g) was collected as the residue by filtration.

[0051] Next, tert-butylindanofleurenone (tBu-FIDO) (1i) was synthesized. First, Dimer (1g) (200.0 mg, 0.112 mmol) was dissolved in o-DCB (20.0 mL), and CuBr was used as an oxidizing agent. 2To the reaction mixture was added tBu-FIDO (1i) (200.0 mg, 0.896 mmol). After vigorously stirring at 135°C for 1 hour, 500 μL of hydrobromic acid (47% hydrogen bromide) was added as the hydrohalic acid. Vigorous stirring was then continued at 135°C for 8 hours. Finally, the reaction mixture was concentrated by evaporating the solvent under vacuum, followed by silica gel column chromatography (CS2) to give tBu-FIDO (1i) (105.2 mg, 53%) as a brownish powder.

[0052] 1i was identified from its H NMR chart (see FIGS. 8 and 9) and C NMR chart (see FIG. 10). The NMR analysis results are shown below.

[0053] 1 H NMR (600MHz, CS 2 / CDCl 3 ) δ8.47 (d, J=1.5Hz, 1H), 8.37 (d, J=8.3Hz, 1H), 7.93 (dd, J=8.3Hz, 1.5Hz, 1H), 1.57 (s, 9H).

[0054] 13C{ 1 H}NMR (125MHz, CS 2 / CDCl 3 , all 2C unless specified) 146.4, 146.4, 146.1, 146.1, 145.9, 145.7, 145.5, 145.5, 145.4, 145.4, 144.7, 144.3, 143.1, 142.8, 142.7, 142.4, 142.2, 142.1, 142.1, 141.9, 141.7, 140.7, 140.6, 135.6, 135.4, 131.7 (1C), 128.3 (1C), 127.1 (1C), 123.0 (1C), 79.2 (1C), 71.1 (1C), 36.0 (1C), 31.2 (3C).

[0055] According to the synthesis reaction of the fullerene derivative represented by the above formula (6) of the present disclosure, as described above, by oxidizing an arylfullerene dimer in the presence of a hydrohalic acid, a fullerene derivative represented by the above formula (6), such as tertiary butylindanoflerenone, can be synthesized in high yield.

[0056] ​Furthermore, in the synthesis reaction of the fullerene derivative represented by the above formula (6) of the present disclosure, by using hydrobromic acid as the hydrohalic acid as described above, the fullerene derivative represented by the above formula (6), such as tertiary butylindanoflerenone, can be easily synthesized in high yield with good reproducibility.

[0057] Furthermore, in the method for producing a fullerene derivative according to the present disclosure, the fullerene derivative is produced using the synthesis reaction of the fullerene derivative represented by the above formula (6), and the obtained fullerene derivative can form a vapor-deposited film having an amorphous structure, and the vapor-deposited film can maintain the amorphous structure even after annealing or exposure to solvent vapor.

[0058] The synthesis reaction of the fullerene derivative of the present disclosure is not limited to the production of fullerene derivatives represented by the above formula (6), such as tertiary butyl indanofullerenone. That is, by preparing an aryl fullerene dimer or a Grignard reagent, fullerene derivatives other than the fullerene derivative represented by the above formula (1), such as indanofullerenone, methyl indanofullerenone, methoxy indanofullerenone, fluoro indanofullerenone, and [6,6]-phenyl-C, which will be described later, can be produced. 61 It can also be applied to the production of butyric acid methyl ester, etc.

[0059] The synthesis reaction of the fullerene derivative is, for example, a synthesis reaction of a fullerene derivative having an indanoflurane thioketone structure (when Y is sulfur) among the fullerene derivatives of the above formula (1). This reaction is a synthesis reaction of a fullerene derivative represented by the following formula (7), in which the fullerene derivative obtained by the synthesis reaction of the fullerene derivative represented by the above formula (6) is reacted with a thionating agent.

[0060]

[0061] The thiolating agent is not particularly limited, and examples thereof include 2,4-bis(4-methoxyphenyl)-1,3-dithia-2,4-diphosphetane 2,4-disulfide (hereinafter referred to as Lawesson's reagent), diphosphorus pentasulfide, etc. Among these, Lawesson's reagent is preferred in terms of efficient conversion of a carbonyl group to a thiocarbonyl group.

[0062] The synthesis reaction of the fullerene derivative represented by the above formula (7) will be specifically described below. Figure 39 shows a synthesis route for tertiary indanoflurane thioketone (tBu-FIDS).

[0063] As shown in FIG. 39, a mixture of tBu-FIDO(A) (210 mg, 0.238 mmol) and Lawesson's reagent (1350 mg, 3.341 mmol) in 50 mL of dry toluene was added to N 2 The mixture was stirred under atmospheric pressure at 120°C for 24 hours. After cooling to room temperature, the reaction mixture was poured into 300 ml of methanol to precipitate the crude product. The filtered crude product was then extracted with CS as an eluent. 2 Silica gel column chromatography using HCl gave tBu-FIDS(B) (80 mg, 37%) as a reddish-brown solid.

[0064] The obtained tBu-FIDS was identified from the H NMR chart (see FIG. 40) and the C NMR chart (see FIGS. 41 and 42). The NMR analysis results are shown below.

[0065] 1H NMR (600MHz, CS 2 / CDCl 3 ).

[0066] 13C NMR (125MHz, CS 2 / CDCl 3 , all 2C unless otherwise specified).

[0067] According to the synthesis reaction of the fullerene derivative represented by the above formula (7) of the present disclosure, as described above, the fullerene derivative obtained in the synthesis reaction of the fullerene derivative represented by the above formula (6) is reacted with a thiolating agent, whereby the fullerene derivative represented by the above formula (7), such as tertiary butyl indanoflurane thioketone, can be synthesized in high yield.

[0068] Furthermore, in the method for producing a fullerene derivative according to the present disclosure, the fullerene derivative is produced using a synthesis reaction of the fullerene derivative represented by the above formula (7), and the obtained fullerene derivative can form a vapor-deposited film having an amorphous structure.

[0069] <Electrical Properties of Fullerene Derivatives> FIG. 11 is a graph showing the reduction potentials of fullerenes and fullerene derivatives. FIG. 12 shows the reduction potential (E 1/2 1 is a table showing the electron affinity (LUMO Level (eV)) of the cations of the cations.

[0070] In Figures 11 and 12, Fc / Fc + is a ferrocene / ferricinium ion standard electrode, C 60 is fullerene (see Figure 13), PC 61 BM is [6,6]-phenyl-C 61 -butyric acid methyl ester (see Figure 27), H-FIDO represents indanofullerenone (see Figure 14), MeO-FIDO represents methoxyindanofullerenone (see Figure 15), F-FIDO represents fluoroindanofullerenone (see Figure 16), Me-FIDO represents methylindanofullerenone (see Figure 17), and tBu-FIDO represents tert-butylindanofullerenone (see Figure 1).

[0071] 11 and 12, tBu-FIDO has an electron affinity of −3.68, which indicates electrical properties equivalent to those of fullerene and fullerene derivatives other than tBu-FIDO (electron affinities of −3.72 to −3.64).

[0072] By utilizing such electrical properties, fullerene derivatives such as tBu-FIDO (FIG. 1, FIGS. 14 to 17, and FIG. 27) can be applied to organic semiconductor materials and devices such as organic light-emitting diodes (OLEDs), organic solar cells (OSCs), and organic photodetectors (OPDs).

[0073] Figure 45 shows fullerene (C 6046 is a graph showing the reduction potentials of C, tertiary butyl indanoflurane (tBu-FIDO), and tertiary butyl indanoflurane thioketone (tBu-FIDS). 60 , tBu-FIDO, and tBu-FIDS reduction potentials (E 1/2 1 is a table showing the electron affinity (LUMO Level (eV)) of the cations of the cations.

[0074] 45 and 46, tBu-FIDI (electron affinity of -3.63) exhibits electrical properties equivalent to those of C60 (electron affinity of -3.74) and tBu-FIDO (electron affinity of -3.66).

[0075] Figure 47 shows C 60 47 is a graph showing the simulated and measured values ​​of the electron affinity of tBu-FIDO and tBu-FIDS. Here, the simulated values ​​are theoretical values ​​of the electron affinity obtained by first-principles band calculation. From FIG. 47, C 60 The experimentally measured electron affinities of tBu-FIDO and tBu-FIDS have been shown to correspond to the theoretical values.

[0076] <Deposit and method for producing the deposit> The deposit of the present disclosure is formed by depositing the fullerene derivative of the present disclosure described above. The formed deposit contains the fullerene derivative of the present disclosure. Furthermore, the method for producing the deposit of the present disclosure is obtained by depositing the fullerene derivative obtained by the method for producing the fullerene derivative of the present disclosure described above. Note that the deposit refers to a substance formed by deposition on a deposition target such as a substrate.

[0077] As a deposition method, known film formation methods can be used, such as physical vapor deposition (PVD) methods such as vacuum deposition, sputtering, ion plating, etc., and chemical vapor deposition (CVD) methods such as thermal CVD, plasma CVD, photo CVD, etc. The deposition material of the present disclosure can be obtained by heating the fullerene derivative of the present disclosure to a temperature equal to or higher than the sublimation temperature and depositing it.

[0078] Here, the deposition product of the present disclosure (deposition product containing tBu-FIDO) and fullerene (C60 The results of X-ray diffraction are compared between a deposition containing tBu-FIDO and a deposition containing a fullerene derivative other than tBu-FIDO, such as H-FIDO or Me-FIDO. 60 The deposited material of H-FIDO and Me-FIDO before annealing is crystalline (see FIG. 18), while the deposited material of H-FIDO and Me-FIDO before annealing is amorphous (see FIGS. 19 and 20). In contrast, the deposited material of tBu-FIDO before annealing is amorphous (see FIG. 21). Here, the amorphous state refers to a state that does not exhibit crystallinity.

[0079] In the X-ray diffraction graphs shown in Figures 19 to 21, if a diffraction peak can be confirmed, the deposited material is determined to be crystalline, and if no diffraction peak can be confirmed, the deposited material is determined to be in an amorphous state.

[0080] In this way, the deposition material of the present disclosure can be formed by depositing the fullerene derivative of the present disclosure, and the deposition material containing a fullerene skeleton can be made amorphous, similar to fullerene derivatives such as H-FIDO and Me-FIDO.

[0081] 26 to 30 show fullerene (C 60 31 shows the results of TGA of the fullerene derivative. In general, the thermal decomposition temperature of a sample is measured in the thermogravimetric analysis, but when the sample is sublimable, the temperature measured as the thermal decomposition onset (1st loss) temperature is the sublimation temperature of the sample.

[0082] Comparing the sublimation temperatures, C 60 is approximately 615°C (see Figure 26), and [6,6]-phenyl-C 61 -Butyric acid methyl ester (PC 61BM) is about 380°C (see FIG. 27), indanofullerenone (H-FIDO) is about 577°C (see FIG. 28), methylindanofullerenone (Me-FIDO) is about 570°C (see FIG. 29), and tertiary butylindanofullerenone (tBu-FIDO) is about 470°C (see FIG. 30). From these TGAs, it can be seen that the fullerene derivative (tBu-FIDO) of the present disclosure has a high affinity for fullerene (C) as well as other fullerene derivatives. 60 ) exhibits a lower sublimation temperature.

[0083] As described above, the deposition material of the present disclosure, formed by depositing the fullerene derivative of the present disclosure, can be deposited at a lower temperature than existing fullerenes or fullerene derivatives as a deposition material containing a fullerene skeleton, similar to fullerene derivatives such as H-FIDO and Me-FIDO, etc. Therefore, the deposition material of the present disclosure is expected to reduce the manufacturing costs of elements or devices using fullerene derivatives.

[0084] The deposition product of the present disclosure can form a film with an amorphous structure. This film with an amorphous structure contains the fullerene derivative of the present disclosure. The film with an amorphous structure can be formed by the known film formation method described above.

[0085] The deposits of the present disclosure do not exhibit crystallinity upon annealing, where "not exhibiting crystallinity" indicates that the deposits are in an amorphous state.

[0086] The annealing test is a test in which a sample is annealed and the crystallinity is evaluated, as will be described in the experimental examples below. The annealing is, for example, a heat treatment at 150°C for 20 minutes in a nitrogen atmosphere. The crystallinity is evaluated by, for example, grazing incidence X-ray diffraction, as shown in Figures 18 to 21.

[0087] Here, when the film of the deposited material (deposited film) is annealed at 150° C., the state of the deposited film (tBu-FIDO) of the present disclosure and the state of fullerene (C 60The states of a vapor-deposited film containing FLN, H-FIDO, and Me-FIDO are compared based on the results of X-ray diffraction. The vapor-deposited films of FLN, H-FIDO, and Me-FIDO (after annealing) exhibit crystalline properties (see FIGS. 18 to 20). In contrast, the vapor-deposited film of tBu-FIDO (after annealing) exhibits an amorphous state (see FIG. 21). That is, the X-ray diffraction results of FIGS. 18 to 21 show that the vapor-deposited film of the fullerene derivative (tBu-FIDO) of the present disclosure maintains an amorphous state even after annealing.

[0088] Comparing the transmission electron microscope (TEM) images in Figures 22 to 25, the deposited film of H-FIDO was amorphous before annealing (see Figure 23), but crystallized after annealing at 150°C (see Figure 25). In contrast, the deposited film of tBu-FIDO was amorphous before annealing (see Figure 22), and maintained its amorphous state even after annealing at 150°C (see Figure 24). That is, the TEM images in Figures 22 to 25 also show that the deposited film of the fullerene derivative (tBu-FIDO) of the present disclosure maintained its amorphous state even after annealing. The same is true for the X-ray diffraction images in Figures 19 and 21. Note that in the TEM images shown in Figures 22 to 25, if the image pattern is regular, the deposited material is judged to be crystalline, and if the image pattern is irregular, the deposited material is judged to be amorphous.

[0089] As described above, the deposition material of the present disclosure forms a film with an amorphous structure, and thus the fullerene derivative can be deposited in an amorphous state. Therefore, the deposition material of the present disclosure can form a film of the fullerene derivative with high uniformity.

[0090] Furthermore, as described above, the deposition material of the present disclosure does not exhibit crystallinity in the annealing test, and therefore the deposition material, which is amorphous before annealing, can maintain the amorphous state after annealing. Therefore, the film of the present disclosure can be used to form a film of an organic element using a fullerene derivative, and is expected to be applied to semiconductor materials and devices.

[0091] Furthermore, in the method for producing a deposition material according to the present disclosure, a deposition material is obtained by depositing the fullerene derivative obtained by the method for producing a fullerene derivative according to the present disclosure, and therefore the deposition temperature of the obtained deposition material is lower than that of existing fullerenes or fullerene derivatives. Therefore, the method for producing a deposition material according to the present disclosure is expected to reduce the production costs of elements or devices using the obtained fullerene derivative.

[0092] FIG. 43 shows a chart of differential thermal analysis (DTA) of tBu-FIDS. From FIG. 43, it can be seen that no endothermic peak is observed from the DTA before 614°C. It can also be seen that the weight of tBu-FIDS rapidly decreases from 440°C onwards. This indicates that tBu-FIDS begins to sublime or its structure decomposes at 440°C. It can also be seen that tBu-FIDS begins to decompose from 614°C onwards.

[0093] Figure 44 shows tBu-FIDS, C 60 44 shows the results of thermogravimetry (TG) of tBu-FIDS and tBu-FIDO. From FIG. 44, it can be seen that the sublimation temperature of tBu-FIDS (420°C) is lower than that of H-FIDO (457°C) or C60 (495°C). In addition, tBu-FIDS undergoes a second weight loss from 460°C, which indicates structural decomposition. Furthermore, the temperature range during weight loss due to sublimation of tBu-FIDS is C 60 , and it can be seen that it is narrower than tBu-FIDO.

[0094] As described above, with the deposition material of the present disclosure, even when tBu-FIDS is deposited, the deposition temperature can be lower than that of fullerene or tBu-FIDO, and therefore it is expected that the manufacturing cost of elements or devices using tBu-FIDS can be reduced.

[0095] Furthermore, in the method for producing a deposition product, even when tBu-FIDS is used, the deposition temperature can be lowered for tBu-FIDS than for fullerene or tBu-FIDO, and therefore it is expected that the production cost of an element or device using tBu-FIDS can be reduced.

[0096] The present disclosure will be further explained below using experimental examples. Various tests and evaluations were carried out according to the following methods.

[0097] [Experimental Example 1] Tertiary butyl indanoflerenone (tBu-FIDO) was used as a fullerene derivative (see Fig. 1 and Fig. 30). In this example, tertiary butyl indanoflerenone may be referred to as tert-butyl fullerene ketone.

[0098] [Experimental Example 2] Instead of a fullerene derivative, fullerene (hereinafter referred to as FLN or C 60 (See Figures 13 and 26).

[0099] Experimental Example 3 Indanofullerenone (H-FIDO) was used as the fullerene derivative (see FIGS. 14 and 28). In this example, indanofullerenone may be referred to as fullerene ketone.

[0100] Experimental Example 4 Methylindanoflerenone (Me-FIDO) was used as the fullerene derivative (see FIGS. 17 and 29).

[0101] Experimental Example 5 Fluoroindanofullerenone (F-FIDO) was used as the fullerene derivative (see FIG. 16).

[0102] Experimental Example 6 Methoxyindanoflerenone (MeO-FIDO) was used as the fullerene derivative (see FIG. 15).

[0103] [Experimental Example 7] As a fullerene derivative, [6,6]-phenyl-C 61 -Butyric acid methyl ester (PC 61 BM) was used (see Figure 27).

[0104] <Deposit> Using a vacuum deposition device (ULVAC VTS-350M), a deposition was carried out under high vacuum (4.76 × 10 -3 The current value of the heater that heated the crucible containing the material to be evaporated was gradually increased at a pressure of 1000 kJ / cm2 (Pa) to sublimate the material, thereby forming a vapor-deposited film of approximately 50 nm. The current value applied when the vapor-deposited film began to form is shown in FIG.

[0105] <Annealing Treatment> The film-formed sample was heat-treated at 150°C for 20 minutes in a nitrogen atmosphere. Specifically, in a nitrogen-substituted glove box, the sample formed on the quartz substrate was placed on a hot plate heated to 150°C, covered with a petri dish, and heat-treated for 20 minutes. When annealing in solvent vapor, the sample and a small bottle containing chlorobenzene as a solvent were placed in the petri dish, and heat-treated at 150°C for 20 minutes.

[0106] <X-ray Diffraction> A sample film of about 30 nm thickness formed on a quartz substrate was set in a thin film X-ray diffractometer (ATX-G manufactured by RIGAKU Corporation) and measured by grazing incidence X-ray diffraction.

[0107] The results of X-ray diffraction showed that in Experimental Example 1 (tBu-FIDO), the deposit before annealing was amorphous and remained amorphous even one month after deposition (see FIGS. 21, 33, and 34). The deposit after annealing was amorphous and remained amorphous even one month after annealing (see FIGS. 21 and 34). Furthermore, the deposit after annealing in solvent vapor was amorphous and remained amorphous even one month after annealing (see FIG. 34).

[0108] On the other hand, in Experimental Example 2 (FLN), the deposition before annealing was crystalline and remained crystalline even one month after deposition (see FIGS. 21, 33, and 35). The deposition after annealing was crystalline and remained crystalline even one month after annealing (see FIGS. 21 and 34). Furthermore, the deposition after annealing in solvent vapor was crystalline and remained crystalline even one month after annealing (see FIG. 35).

[0109] In both Experimental Example 3 (H-FIDO) and Experimental Example 4 (Me-FIDO), the deposited material before annealing was amorphous, and the deposited material after annealing was crystalline (see FIGS. 19 and 20).

[0110] These results demonstrate that the fullerene derivative of Experimental Example 1 (tBu-FIDO) maintains the amorphous state immediately after deposition even after annealing, and that the amorphous state before and after annealing can be maintained for a long period of time regardless of whether the fullerene derivative is in solvent vapor or not. Therefore, the fullerene derivative of Experimental Example 1 (tBu-FIDO) facilitates the formation of films of organic elements and the like using fullerene derivatives, and is expected to be applied to semiconductor materials and devices, etc.

[0111] <Transmission Electron Microscope (TEM) Image> The sample formed on the quartz substrate was set in a transmission electron microscope, and TEM measurement was performed.

[0112] From the TEM images, in Experimental Example 1 (tBu-FIDO), the deposit was amorphous before annealing (see FIG. 22) and after annealing (see FIG. 24). In contrast, in Experimental Example 3 (H-FIDO), the deposit was amorphous before annealing (see FIG. 23) and after annealing (see FIG. 25).

[0113] The results of this TEM image also show that the fullerene derivative of Experimental Example 1 (tBu-FIDO) maintains the amorphous state immediately after deposition even after annealing, and is a fullerene derivative that can be easily used to form films of organic devices and the like using the fullerene derivative.

[0114] <Thermogravimetric analysis (TGA)> Approximately 5 mg of sample was placed in a thermogravimetric analyzer (Shimadzu Corporation, DTG-60AH). The temperature was raised from room temperature to 100°C at a rate of 10°C / min under a nitrogen stream and held at that temperature for 10 minutes. The temperature was then raised from 100°C to 1000°C at a rate of 10°C / min, and the change in weight was measured. Figures 26 to 30 show the results from 100°C onwards.

[0115] From the results of TGA, the sublimation temperature of the deposited material was 471.41°C in Experimental Example 1 (tBu-FIDO) (see Figures 30 and 31). 60 ) was 615.17°C, Experimental Example 3 (H-FIDO) was 569.92°C, Experimental Example 4 (Me-FIDO) was 577.46°C, and Experimental Example 7 (PC 61BM) was 380.26°C (see Figures 26 to 29 and Figure 31).

[0116] From this result, it can be seen that the fullerene derivative of Experimental Example 1 (tBu-FIDO) has the same properties as existing fullerene derivatives, and is capable of producing fullerene (C 60 ) and the deposition temperature was found to be lower than that of the fullerene derivative of Experimental Example 1 (tBu-FIDO). Therefore, the fullerene derivative of Experimental Example 1 (tBu-FIDO) has the same properties as the existing fullerene derivatives, and 60 ), the deposition temperature can be lowered, and it is expected that the manufacturing cost of elements or devices using fullerene derivatives will be reduced.

[0117] <Thermogravimetric measurement (vacuum TG)> A sample (approximately 5 mg) was placed in a vacuum thermogravimetric analyzer (TG / DTA6200 manufactured by Hitachi High-Tech Science Corporation). In a vacuum of 1 Pa or less, the sample was heated from room temperature to 1000°C at a rate of 10°C / min, and the change in weight was measured.

[0118] From the results of vacuum TG, Experimental Example 1 (tBu-FIDO) was found to be superior to Experimental Example 2 (C 60 ) and Experimental Example 3 (H-FIDO), it was found that weight loss due to sublimation began earlier (see FIG. 37).

[0119] These results demonstrate that the fullerene derivative of Experimental Example 1 (tBu-FIDO) takes less time to sublimate than existing fullerenes or fullerene derivatives under the same temperature increase. Therefore, the fullerene derivative of Experimental Example 1 (tBu-FIDO) can be vapor deposited in a shorter time than existing fullerenes or fullerene derivatives, which is expected to reduce the manufacturing costs of elements or devices using fullerene derivatives.

[0120] <Measurement of Current During Sublimation> When producing the above-described deposition material, the current value applied to the crucible was measured, and the current value at which the deposition film started to form was taken as the current during sublimation (see FIG. 32).

[0121] The current during sublimation was 70 A in Experimental Example 1 (tBu-FIDO). 60) was 90 A, and in Experimental Example 3 (H-FIDO) it was 110 A (see FIG. 32). From these results, it is expected that the fullerene derivative of Experimental Example 1 (tBu-FIDO) will have a lower sublimation temperature than existing fullerenes or fullerene derivatives.

[0122] Therefore, the fullerene derivative of Experimental Example 1 (tBu-FIDO) can be vapor deposited at a lower temperature and for a shorter time than conventional fullerenes or fullerene derivatives, and this is expected to reduce the manufacturing costs of elements or devices using fullerene derivatives.

[0123] <Ultraviolet-Visible Spectroscopy (UV-vis)> A sample formed into a film of about 30 nm on a quartz substrate was set in a UV-visible spectrophotometer (V-650 manufactured by JASCO Corporation) and measured in the wavelength range of 200 to 900 nm.

[0124] From the results of ultraviolet-visible spectroscopy, for example, at a wavelength of 450 nm (blue), the absorbance of Experimental Example 1 (tBu-FIDO) was about 0.2 (see FIG. 36). 60 The absorbance of the HCl solution was approximately 0.3 (see FIG. 36).

[0125] From this result, it can be said that the fullerene derivative of Experimental Example 1 (tBu-FIDO) has the property of being less absorbing blue wavelengths than fullerene, and therefore the deposited material of Experimental Example 1 (tBu-FIDO) can be used, for example, as an acceptor in an image sensor.

[0126] Although the embodiments of the present invention have been described above, the present invention is not limited to the specific embodiments, and various modifications and changes are possible within the scope of the invention described in the claims.

[0127] This application claims priority based on Japanese Patent Application No. 2023-048815 filed on March 24, 2023 and Japanese Patent Application No. 2023-205171 filed on December 5, 2023, the entire contents of which are incorporated herein by reference.

Claims

1. Formula (1) (wherein FLN is a fullerene skeleton, X is a halogen group or an organic group, and Y is O or S).

2. Formula (2) 2. The fullerene derivative according to claim 1, represented by the formula: (wherein tBu is a tertiary butyl group).

3. Formula (3) The fullerene derivative according to claim 2 , represented by:

4. Formula (4) 2. The fullerene derivative according to claim 1, represented by the formula: (wherein tBu is a tertiary butyl group).

5. Formula (5) The fullerene derivative according to claim 4 , represented by:

6. The fullerene skeleton is C 60 Skeleton, C 70 Skeleton, C 76 Skeleton, and C 78 The fullerene derivative according to claim 1 , wherein the fullerene derivative is at least one selected from the group consisting of a cyclic alkyl group, ...

7. A deposit formed by depositing the fullerene derivative according to any one of claims 1 to 6.

8. The deposition product according to claim 7, which is a film having an amorphous structure.

9. The deposition material according to claim 7 or 8, which does not show crystallinity in the following annealing test: The deposition material is heat-treated at 150° C. for 20 minutes in a nitrogen atmosphere, and the crystallinity is evaluated by grazing incidence X-ray diffraction.

10. Oxidizing an aryl fullerene dimer in the presence of a hydrohalic acid, formula (6): (wherein FLN is a fullerene skeleton, and X is hydrogen, a halogen group, or an organic group).

11. The synthesis reaction of a fullerene derivative according to claim 10, wherein the hydrohalic acid is hydrobromic acid.

12. The fullerene derivative obtained by the synthesis reaction according to claim 10 or 11 is reacted with a thiolation agent, (wherein FLN is a fullerene skeleton, and X is a halogen group or an organic group).

13. A method for producing a fullerene derivative, comprising the steps of: producing the fullerene derivative by using the synthesis reaction according to any one of claims 10 to 12.

14. A method for producing a deposition product, comprising obtaining a fullerene derivative by the production method according to claim 13, and depositing the fullerene derivative to obtain a deposition product.

Citation Information

Patent Citations

  • Photoelectric conversion element, method for producing fullerene compound, and fullerene compound

    JP2012094829A

  • Fullerene derivatives, and thin film, photoelectric element, image sensor and electronic device comprising the same

    JP2019099570A

  • Fullerene derivative, fullerene derivative production method, deposit, film, and electronic device

    WO2021149801A1