Method for producing stretched film

The described method for heat-treating poly(3-hydroxybutyrate) resin-based stretched films addresses heat shrinkage issues by applying a non-contact heating method with controlled relaxation, improving their stability and applicability in thermal applications.

WO2024203640A1PCT designated stage expired Publication Date: 2024-10-03KANEKA CORP

Patent Information

Application Number
PCT/JP2024/010810
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-09-21
Filing Date
2024-03-19
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Poly(3-hydroxybutyrate) resin-based stretched films exhibit significant heat shrinkage, which complicates their use in applications like packaging and printing due to distortion issues when heated, as they shrink and lose dimensional stability.

Method used

A method involving melting poly(3-hydroxybutyrate) resin in an extruder, forming it into a film, stretching it, and then heat-treating it using a non-contact heating method with a specific relaxation amount of 9 to 50% in a specific direction, below the melting point of the resin, to minimize heat shrinkage.

Benefits of technology

The method effectively reduces heat shrinkage in poly(3-hydroxybutyrate) resin-based stretched films, enhancing their dimensional stability and usability in applications requiring thermal processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010810_03102024_PF_FP_ABST
    Figure JP2024010810_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a method for producing a stretched film containing a poly(3-hydroxybutyrate)-based resin and having low heat shrinkage. Specifically provided is a method for producing a stretched film containing a poly(3-hydroxybutyrate)-based resin, the method comprising: a step for melting a film raw material containing the poly(3-hydroxybutyrate)-based resin using an extruder and then molding a molten product into a film; a step for stretching the molded film in a specific direction; and a step for subjecting the stretched film to a heat treatment. In the method, the heat treatment comprises employing a non-contact heating method to heat the stretched film to a temperature that is equal to or higher than a temperature (°C) lower by 40°C than the melting point of the (poly(3-hydroxybutyrate)-based resin and that is equal to or lower than the melting point (°C) of the poly(3-hydroxybutyrate)-based resin, at a relaxation amount in the specific direction of 9 to 50%, wherein the relaxation amount is expressed by formula (i). Relaxation amount [%] = \{(the size of the film in the specific direction before the heat treatment)-(the size of the film in the specific direction during the heat treatment)\} / (the size of the film in the specific direction before the heat treatment)×100 (i)
Need to check novelty before this filing date? Find Prior Art

Description

Stretched film manufacturing method

[0001] The present invention relates to a method for producing a stretched film containing a poly(3-hydroxybutyrate)-based resin.

[0002] In recent years, the separate collection and composting of food waste has been promoted, particularly in Europe, and there is a demand for plastic products that can be composted together with food waste.

[0003] On the other hand, environmental problems caused by discarded plastics have been highlighted, and it has become clear that large amounts of plastic, particularly plastics dumped in the ocean or that have entered the ocean via rivers, are drifting in the ocean on a global scale. Because such plastics retain their shape for a long period of time, they can trap and capture marine organisms, a phenomenon known as ghost fishing, and if ingested by marine organisms, they can become trapped in the digestive tract, causing feeding disorders, and other problems have been pointed out as having an impact on the ecosystem.

[0004] Furthermore, it has been pointed out that microplastics, which are plastics that have broken down and become tiny particles due to ultraviolet rays and other factors, absorb harmful compounds in seawater, and when marine organisms ingest these, the harmful substances are absorbed into the food chain.

[0005] The use of biodegradable plastics is expected to address this type of marine pollution caused by plastics, but a report compiled by the United Nations Environment Programme in 2015 pointed out that plastics that can be biodegraded through compost, such as polylactic acid, cannot be expected to decompose in a short period of time in the cold ocean, and therefore cannot be used to combat marine pollution.In this context, poly(3-hydroxybutyrate) resins are attracting attention as a material that can resolve the above issues, as they are capable of biodegrading even in seawater.

[0006]

[0003] Meanwhile, a method of stretching a film is known as a technique for producing a thin, high-strength film. For example, to produce a stretched film from a general-purpose resin such as polypropylene, a molten resin is cooled and solidified using a cast roll to form a raw sheet, and the raw sheet is then preheated to a temperature at which it can be stretched, and then stretched, thereby enabling continuous production of the stretched film with good productivity.

[0007] However, poly(3-hydroxybutyrate)-based resins are known to be difficult to stretch due to their properties. Patent Document 1 discloses a method for producing a biaxially stretched film containing a poly(3-hydroxybutyrate)-based resin with high productivity.

[0008] JP 2022-062759 A JP 2006-145912 A

[0009] When a stretched film containing a poly(3-hydroxybutyrate)-based resin as a main component is used, for example, as a packaging film, it is subjected to heat bonding between stretched films to seal the contents, or heat fixation of ink applied to the stretched film for printing. However, such heating causes a problem that the stretched film shrinks, distorting the sealed portion or the printing.

[0010] Patent Document 2 discloses that a reflective film containing an aliphatic polyester resin, an acrylic resin, and a fine powder filler is heat-treated at 90°C to 160°C after stretching in order to impart dimensional stability to the film. However, even if a similar heat treatment is performed on a stretched film containing a poly(3-hydroxybutyrate) resin, heat shrinkage cannot be sufficiently suppressed.

[0011] In view of the above-mentioned current situation, an object of the present invention is to provide a method for producing a stretched film containing a poly(3-hydroxybutyrate) resin, which has little heat shrinkage.

[0012] As a result of intensive research aimed at solving the above problems, the present inventors have found that a stretched film containing a poly(3-hydroxybutyrate)-based resin with little heat shrinkage can be produced by stretching a film containing a poly(3-hydroxybutyrate)-based resin and then heat-treating it under specific conditions, thereby completing the present invention.

[0013] That is, the present invention relates to a method for producing a stretched film containing a poly(3-hydroxybutyrate)-based resin, the method comprising the steps of melting a film raw material containing the poly(3-hydroxybutyrate)-based resin in an extruder and then forming the film into a film, stretching the formed film in a specific direction, and heat-treating the stretched film, wherein the heat treatment is a treatment in which the stretched film is heated by a non-contact heating method to a temperature of (melting point of the poly(3-hydroxybutyrate)-based resin - 40)°C or higher and (melting point of the poly(3-hydroxybutyrate)-based resin)°C or lower, with a relaxation amount in the specific direction of 9 to 50%, as represented by the following formula (i): Relaxation amount [%] = {(film dimension in the specific direction before heat treatment) - (film dimension in the specific direction during heat treatment)} / (film dimension in the specific direction before heat treatment) × 100 (i)

[0014] According to the present invention, a method for producing a stretched film containing a poly(3-hydroxybutyrate) resin, which has little heat shrinkage, can be provided.

[0015] 1 is a diagram illustrating the concept of the amount of relaxation of a film.

[0016] Although embodiments are described below, the present invention is not limited to the following embodiments. This embodiment relates to a method for producing a stretched film containing a poly(3-hydroxybutyrate)-based resin, the method comprising the steps of melting a film raw material containing the poly(3-hydroxybutyrate)-based resin in an extruder and then forming the film into a film, stretching the formed film in a specific direction, and heat-treating the stretched film, wherein the heat treatment is a treatment in which the stretched film is heated by a non-contact heating method to a temperature between (melting point of poly(3-hydroxybutyrate)-based resin - 40)°C and (melting point of poly(3-hydroxybutyrate)-based resin)°C, with a relaxation amount in the specific direction of 9 to 50% as represented by the following formula (i): Relaxation amount [%] = {(film dimension in the specific direction before heat treatment) - (film dimension in the specific direction during heat treatment)} / (film dimension in the specific direction before heat treatment) × 100 (i)

[0017] <Poly(3-hydroxybutyrate)-based Resin> The poly(3-hydroxybutyrate)-based resin is an aliphatic polyester-based resin that can be produced from a microorganism and is a polyester resin containing 3-hydroxybutyrate as a repeating unit. The poly(3-hydroxybutyrate)-based resin may be a poly(3-hydroxybutyrate) containing only 3-hydroxybutyrate as a repeating unit, or may be a copolymer of 3-hydroxybutyrate and another hydroxyalkanoate. Furthermore, the poly(3-hydroxybutyrate)-based resin may be a mixture of a homopolymer and one or more copolymers, or a mixture of two or more copolymers.

[0018] Specific examples of the poly(3-hydroxybutyrate)-based resin include poly(3-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) [hereinafter, may be referred to as P3HB3HH], poly(3-hydroxybutyrate-co-3-hydroxyvalerate) [hereinafter, may be referred to as P3HB3HV], poly(3-hydroxybutyrate-co-4-hydroxybutyrate) [hereinafter, may be referred to as P3HB4HB], poly(3-hydroxybutyrate-co-3-hydroxyoctanoate), poly(3-hydroxybutyrate-co-3-hydroxyoctadecanoate), and the like. Among these, poly(3-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate), and poly(3-hydroxybutyrate-co-4-hydroxybutyrate) are preferred because they are easy to produce industrially.

[0019] Furthermore, poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) is preferred from the viewpoints that by changing the composition ratio of the repeating units, it is possible to change the melting point and degree of crystallinity, and thereby change physical properties such as Young's modulus and heat resistance, making it possible to impart physical properties between those of polypropylene and polyethylene, and that it is easy to produce industrially and is a physically useful plastic. In particular, among poly(3-hydroxybutyrate)-based resins that tend to be thermally decomposed when heated to 180°C or higher, poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) is preferred from the viewpoints that it can lower the melting point and enable molding and processing at low temperatures.

[0020] Commercially available products of poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) include Kaneka Biodegradable Polymer PHBH (registered trademark) manufactured by Kaneka Corporation.

[0021] When the poly(3-hydroxybutyrate) resin contains a copolymer of 3-hydroxybutyrate units and other hydroxyalkanoate units, the average content ratio of 3-hydroxybutyrate units and other hydroxyalkanoate units to all monomer units constituting the poly(3-hydroxybutyrate) resin is preferably 3-hydroxybutyrate units / other hydroxyalkanoates = 99 / 1 to 80 / 20 (mol % / mol %), and more preferably 97 / 3 to 85 / 15 (mol % / mol %), from the viewpoint of achieving both strength and productivity of the stretched film.

[0022] The average content ratio of each monomer unit in all monomer units constituting the poly(3-hydroxybutyrate)-based resin can be determined by a method known to those skilled in the art, for example, the method described in paragraph

[0047] of WO 2013 / 147139. The average content ratio means the molar ratio of each monomer unit in all monomer units constituting the poly(3-hydroxybutyrate)-based resin, and when the poly(3-hydroxybutyrate)-based resin is a mixture of two or more poly(3-hydroxybutyrate)-based resins, it means the molar ratio of each monomer unit contained in the entire mixture.

[0023] The poly(3-hydroxybutyrate) resin may be a mixture of at least two types of poly(3-hydroxybutyrate) resins that differ from each other in the type of constituent monomer and / or the content ratio of the constituent monomer.

[0024] The weight average molecular weight of the entire poly(3-hydroxybutyrate) resin is not particularly limited, but from the viewpoint of achieving both strength and productivity of the stretched film, it is preferably 200,000 to 2,000,000 g / mol, more preferably 250,000 to 1,500,000 g / mol, and even more preferably 300,000 to 1,000,000 g / mol.

[0025] The weight-average molecular weight of the poly(3-hydroxybutyrate) resin can be measured in terms of polystyrene using gel permeation chromatography (HPLC GPC system manufactured by Shimadzu Corporation) using a chloroform solution. As the column for the gel permeation chromatography, a column appropriate for measuring the weight-average molecular weight may be used.

[0026] The method for producing poly(3-hydroxybutyrate) resins is not particularly limited, and may be a production method using chemical synthesis or a production method using a microorganism. Among these, a production method using a microorganism is preferred. Known methods can be applied to the production method using a microorganism. For example, known bacteria that produce copolymers of 3-hydroxybutyrate and other hydroxyalkanoates include Aeromonas caviae, which produces P3HB3HV and P3HB3HH, and Alcaligenes eutrophus, which produces P3HB4HB. In particular, with regard to P3HB3HH, in order to increase the productivity of P3HB3HH, Alcaligenes eutrophus AC32 strain (FERM BP-6038) (T. Fukui, Y. Doi, J. Bateriol., 179, pp. 4821-4830 (1997)) or the like into which genes encoding P3HA (poly(3-hydroxyalkanoate)) synthases have been introduced is more preferred, and microbial cells obtained by culturing these microorganisms under appropriate conditions and allowing P3HB3HH to accumulate within the cells are used. In addition to the above, genetically modified microorganisms into which various poly(3-hydroxybutyrate) resin synthesis-related genes have been introduced may also be used depending on the poly(3-hydroxybutyrate) resin to be produced, or the culture conditions, including the type of substrate, may be optimized.

[0027] The poly(3-hydroxybutyrate) resin may be an unmodified resin, or may be a resin obtained by modifying an unmodified poly(3-hydroxybutyrate) resin with a raw material that reacts with the resin, such as a peroxide (hereinafter referred to as a "modifying raw material").

[0028] When a modified resin is used as a film raw material, a film raw material containing a poly(3-hydroxybutyrate)-based resin that has been previously reacted with a modifying raw material may be molded into a film, or a film raw material containing an unmodified poly(3-hydroxybutyrate)-based resin and a modifying raw material may be molded with the modifying raw material. When reacting a resin with a modifying raw material, the entire resin may be reacted with the modifying raw material, or a portion of the resin may be reacted with the modifying raw material to obtain a modified resin, and the remaining unmodified resin may then be added to the modified resin.

[0029] The modification raw material is not particularly limited as long as it is a compound that can react with the poly(3-hydroxybutyrate)-based resin. However, an organic peroxide is preferably used in terms of ease of handling and ease of controlling the reaction with the poly(3-hydroxybutyrate)-based resin.

[0030] Examples of the organic peroxides include diisobutyl peroxide, cumyl peroxyneodecanoate, di-n-propyl peroxydicarbonate, diisopropyl peroxydicarbonate, di-sec-butyl peroxydicarbonate, 1,1,3,3-tetramethylbutyl peroxyneodecanoate, bis(4-t-butylcyclohexyl)peroxydicarbonate, bis(2-ethylhexyl)peroxydicarbonate, t-hexyl peroxyneodecanoate, t-butyl peroxyneodecanoate, t-butyl peroxyneoheptanoate, t-hexyl peroxypivalate, t-butyl peroxypivalate, di(3,5,5-trimethylhexanoyl)peroxide, dilauroyl peroxide, 1,1,3,3-tetramethylbutylperoxy-2-methyl- t-ethylhexanoate, disuccinic acid peroxide, 2,5-dimethyl-2,5-bis(2-ethylhexanoylperoxy)hexane, t-hexylperoxy-2-ethylhexanoate, di(4-methylbenzoyl)peroxide, dibenzoyl peroxide, t-butylperoxy 2-ethylhexyl carbonate, t-butylperoxy isopropyl carbonate, 1,6-bis(t-butylperoxycarbonyloxy)hexane, t-butylperoxy-3,5,5-trimethylhexanoate, t-butylperoxyacetate, t-butylperoxybenzoate, t-amylperoxy, 3,5,5-trimethylhexanoate, 2,2-bis(4,4-di-t-butylperoxycyclohexyl)propane, 2,2-di-t-butylperoxybutane, and the like. Among these, t-butylperoxy 2-ethylhexyl carbonate and t-butylperoxy isopropyl carbonate are preferred. Furthermore, a combination of two or more of these organic peroxides can also be used.

[0031] The organic peroxide is used in various forms such as solid or liquid, and may be in liquid form diluted with a diluent, etc. Among these, an organic peroxide in a form that can be easily mixed with the poly(3-hydroxybutyrate)-based resin (particularly an organic peroxide that is liquid at room temperature (25°C)) is preferred because it can be more uniformly dispersed in the poly(3-hydroxybutyrate)-based resin and is likely to suppress local modification reactions in the resin composition.

[0032] The content of the poly(3-hydroxybutyrate) resin in the stretched film may be 50% by weight or more, 55% by weight or more, 60% by weight or more, 70% by weight or more, or 80% by weight or more. The upper limit of the content of the poly(3-hydroxybutyrate) resin is not limited, and may be 100% by weight or less.

[0033] The stretched film may contain additives that can be used with the poly(3-hydroxybutyrate)-based resin, provided that the effects of the invention are not impaired. Examples of such additives include colorants such as pigments and dyes, odor absorbers such as activated carbon and zeolite, fragrances such as vanillin and dextrin, fillers, plasticizers, antioxidants, weather resistance improvers, UV absorbers, crystal nucleating agents, lubricants, release agents, water repellents, antibacterial agents, and sliding properties improvers. The film may contain only one type of additive, or two or more types. The content of these additives can be appropriately determined by those skilled in the art depending on the intended use. Even when the poly(3-hydroxybutyrate)-based resin contains these additives, its melting point is approximately the same as that of the poly(3-hydroxybutyrate)-based resin.

[0034] The crystal nucleating agent, lubricant, filler, and plasticizer will be described in more detail below. (Crystal Nucleating Agent) Examples of crystal nucleating agents include polyhydric alcohols such as pentaerythritol, galactitol, and mannitol; orotic acid, aspartame, cyanuric acid, glycine, zinc phenylphosphonate, and boron nitride. Among these, pentaerythritol is preferred because of its particularly excellent effect of promoting the crystallization of poly(3-hydroxybutyrate) resins. One or more crystal nucleating agents may be used, and the ratio of their use can be appropriately adjusted depending on the purpose.

[0035] The amount of the nucleating agent used is not particularly limited, but is preferably 0.1 to 5 parts by weight, more preferably 0.5 to 3 parts by weight, and even more preferably 0.7 to 1.5 parts by weight, per 100 parts by weight of the total amount of the poly(3-hydroxybutyrate) resin.

[0036] (Lubricant) Examples of lubricants include behenamide, oleamide, erucamide, stearamide, palmitamide, N-stearylbehenamide, N-stearylerucamide, ethylenebisstearamide, ethylenebisoleamide, ethylenebiserucamide, ethylenebislauricamide, ethylenebiscapricamide, p-phenylenebisstearamide, and polycondensates of ethylenediamine, stearic acid, and sebacic acid. Among these, behenamide or erucamide is preferred because of its particularly excellent lubricating effect on poly(3-hydroxybutyrate)-based resins. One or more types of lubricants may be used, and the ratio of use can be appropriately adjusted depending on the purpose.

[0037] The amount of the lubricant used is not particularly limited, but is preferably 0.01 to 5 parts by weight, more preferably 0.05 to 3 parts by weight, and even more preferably 0.1 to 1.5 parts by weight, per 100 parts by weight of the total amount of the poly(3-hydroxybutyrate) resin.

[0038] (Filler) By including a filler, a stretched film with higher strength can be obtained. The filler may be either an inorganic filler or an organic filler, or both may be used in combination. The inorganic filler is not particularly limited, but examples thereof include silicates, carbonates, sulfates, phosphates, oxides, hydroxides, nitrides, and carbon black. Only one type of inorganic filler may be used, or two or more types may be used in combination.

[0039] The content of the filler is not particularly limited, but is preferably 1 to 100 parts by weight, more preferably 3 to 80 parts by weight, even more preferably 5 to 70 parts by weight, and even more preferably 10 to 60 parts by weight, relative to 100 parts by weight of the total amount of the poly(3-hydroxybutyrate) resin. However, the stretched film does not have to contain a filler.

[0040] (Plasticizers) Examples of plasticizers include glycerin ester compounds, citrate ester compounds, sebacate compounds, adipate compounds, polyether ester compounds, benzoate ester compounds, phthalate ester compounds, isosorbide ester compounds, polycaprolactone compounds, and dibasic acid ester compounds. Among these, glycerin ester compounds, citrate ester compounds, sebacate compounds, and dibasic acid ester compounds are preferred because of their particularly excellent plasticizing effect on poly(3-hydroxyalkanoate) resins. Examples of glycerin ester compounds include glycerin diacetomonolaurate. Examples of citrate ester compounds include acetyl tributyl citrate. Examples of sebacate ester compounds include dibutyl sebacate. Examples of dibasic acid ester compounds include benzyl methyl diethylene glycol adipate. One type of plasticizer may be used, or two or more types may be used, and the ratio of use can be adjusted appropriately depending on the purpose.

[0041] The amount of the plasticizer used is not particularly limited, but is preferably 1 to 20 parts by weight, more preferably 2 to 15 parts by weight, and even more preferably 3 to 10 parts by weight, per 100 parts by weight of the total amount of the poly(3-hydroxybutyrate) resin. However, the stretched film does not necessarily need to contain a plasticizer.

[0042] (Other Resins) The stretched film may contain other resins besides the poly(3-hydroxybutyrate)-based resin, provided that the effects of the invention are not impaired. Examples of such other resins include aliphatic polyester-based resins such as poly(3-hydroxypropionate), poly(4-hydroxybutyrate), polybutylene succinate adipate, polybutylene succinate, polycaprolactone, and polylactic acid, and aliphatic aromatic polyester-based resins such as polybutylene adipate terephthalate (PBAT), polybutylene sebate terephthalate, and polybutylene azelate terephthalate. The other resins may be contained alone or in combination.

[0043] The content of the other resin is not particularly limited, but may be 100 parts by weight or less, 80 parts by weight or less, 70 parts by weight or less, 50 parts by weight or less, 30 parts by weight or less, 20 parts by weight or less, 10 parts by weight or less, 5 parts by weight or less, or 1 part by weight or less, relative to 100 parts by weight of the poly(3-hydroxybutyrate)-based resin. The lower limit of the content of the other resin is not particularly limited, and may be 0 parts by weight or more.

[0044] Furthermore, when the other resin has a higher melting point than the poly(3-hydroxybutyrate)-based resin, the lower limit may be 10 parts by weight or more, 20 parts by weight or more, 50 parts by weight or more, or 65 parts by weight or more relative to 100 parts by weight of the poly(3-hydroxybutyrate)-based resin, and the upper limit may be less than 100 parts by weight relative to 100 parts by weight of the poly(3-hydroxybutyrate)-based resin.

[0045] <Production of Stretched Film> A stretched film containing the poly(3-hydroxybutyrate)-based resin of the present disclosure can be produced by the following production method. This production method includes the steps of melting a film raw material containing the poly(3-hydroxybutyrate)-based resin in an extruder and then molding the melted film into a film, stretching the formed film in a specific direction, and heat-treating the stretched film, wherein the heat treatment is a treatment in which the stretched film is heated by a non-contact heating method to a temperature between (melting point of poly(3-hydroxybutyrate)-based resin - 40)°C and (melting point of poly(3-hydroxybutyrate)-based resin)°C, with a relaxation amount in the specific direction of 9 to 50% as represented by the following formula (i): Relaxation amount [%] = {(film dimension in the specific direction before heat treatment) - (film dimension in the specific direction during heat treatment)} / (film dimension in the specific direction before heat treatment) × 100 (i)

[0046] (Molding Step) In the step of melting a film raw material containing a poly(3-hydroxybutyrate) resin in an extruder and then molding it into a film, the method for molding it into a film is not particularly limited, and known manufacturing methods can be used as appropriate. Specific examples include inflation molding, T-die extrusion molding using an extruder equipped with a T-die, calendar molding, and rolling. Among these, inflation molding and T-die extrusion molding are preferred because they allow for the production of strip-shaped films with good productivity. Furthermore, the extruder can be a single-screw extruder (also called a single-screw extruder), a twin-screw extruder, or the like as appropriate.

[0047] The molding temperature is not particularly limited as long as it is a temperature at which the resin can be appropriately melted, but is preferably, for example, from (melting point of poly(3-hydroxybutyrate)-based resin)°C to (melting point of poly(3-hydroxybutyrate)-based resin + 50°C), more preferably from (melting point of poly(3-hydroxybutyrate)-based resin)°C to (melting point of poly(3-hydroxybutyrate)-based resin + 30°C), and even more preferably from (melting point of poly(3-hydroxybutyrate)-based resin)°C to (melting point of poly(3-hydroxybutyrate)-based resin + 20°C). The molding temperature here refers to the resin temperature from after the extruder until it is discharged from the die. The resin temperature can generally be measured, for example, using a thermometer installed in an adapter.

[0048] (Blown-film extrusion method) The blown-film extrusion method is a molding method in which a molten resin is extruded into a tube from an extruder equipped with a cylindrical die at the tip, and immediately thereafter, a gas is blown into the tube to inflate it into a balloon shape to form a film. The blown-film extrusion method is not particularly limited, but can be carried out using, for example, a general blown-film extrusion machine used for forming a thermoplastic resin into a film.

[0049] A typical inflation molding machine is a single-screw extruder equipped with a cylindrical die. The single-screw extruder may be any extruder that melts and kneads the introduced raw resin and maintains the desired temperature while achieving a constant discharge. The screw shape of the single-screw extruder is not particularly limited, but extruders equipped with mixing elements are preferred from the viewpoint of kneading performance. The structure of the cylindrical die is also not particularly limited, but a spiral mandrel die is preferred because it reduces the occurrence of welds and facilitates thickness uniformity.

[0050] In inflation molding, air rings blown from outside the bubble can be used to solidify the discharged molten resin and stabilize the bubble. A suitable air ring blowing structure is a slit type with multiple annular slits for blowing air out and chambers between each slit to promote bubble stabilization.

[0051] The blow-up ratio (hereinafter sometimes referred to as BUR) in inflation molding is the circumferential length of the bubble cross section divided by the die diameter. From the viewpoint of improving film strength, the lower limit of BUR is preferably 1.5 times or more, more preferably 1.7 times or more, even more preferably 1.9 times or more, and particularly preferably 2 times or more. From the viewpoint of molding stability, the upper limit of BUR is preferably 5.5 times or less, more preferably 4.5 times or less, even more preferably 4.0 times or less, and particularly preferably 3.5 times or less.

[0052] (T-die extrusion molding method) The T-die extrusion molding method refers to a molding method in which a resin molten by an extruder is extruded into a film shape from a slit-shaped outlet onto a cast roll to form a film. The T-die is not particularly limited, and any known T-die can be used as appropriate. For example, the T-die preferably has an outlet shaped to be able to extrude a film-shaped raw material, but the shape is not particularly limited. The shape of the outlet is also not particularly limited.

[0053] In the T-die extrusion molding method, a film-shaped raw material is extruded from the discharge port of a T-die. The shape of the raw material may be a film, and the thickness and width are not particularly limited. The thickness is preferably about 20 μm to 600 μm, since this results in less thickness variation and allows for easy cooling after extrusion.

[0054] The melt viscosity of the raw material extruded from the discharge port of the T-die is not particularly limited, but is preferably 1500 Pa sec or less in order to minimize thickness unevenness and prevent the occurrence of die lines. The melt viscosity can be measured according to a known method as appropriate.

[0055] The take-up speed in inflation molding and T-die extrusion molding is determined by the film thickness, width, and resin discharge rate, but can be adjusted within a range that maintains bubble stability. Generally, a speed of 1 to 100 m / min is preferred.

[0056] The thickness of the film before stretching is not particularly limited and may be appropriately set in consideration of the desired thickness of the stretched film, the stretching ratio, strength, etc. For example, the thickness is preferably 20 to 600 μm, more preferably 40 to 500 μm, and even more preferably 50 to 300 μm. The thickness of the film can be measured using a vernier caliper.

[0057] (Stretching Step) In the step of stretching the formed film in a specific direction, the method is not particularly limited as long as the stretching is possible, and known manufacturing methods can be used as appropriate.

[0058] The stretching direction in the stretching step is not particularly limited, and the film can be stretched in any direction in the plane direction. When the stretched film of the present disclosure is a strip-shaped film, the stretching direction may be either the MD direction or the TD direction of the film, or both the MD direction and the TD direction. Stretching in either the MD direction or the TD direction is called uniaxial stretching, and stretching in both the MD direction and the TD direction is called biaxial stretching. Here, the MD direction is also called the machine direction, flow direction, or longitudinal direction. The TD direction is the direction perpendicular to the MD direction, and is also called the perpendicular direction or width direction.

[0059] Although the specific stretching method is not particularly limited, a method of stretching the film by stretching it in the stretching direction is preferred. Stretching the film in the stretching direction means pulling the film in the stretching direction. On the other hand, when stretching is performed by applying pressure in the thickness direction of the film, such as roll rolling in which the film is sandwiched between two rolls, the film tends to adhere to the rolling rolls, which may reduce the productivity of the stretched film.

[0060] The method for stretching the film in the stretching direction is not particularly limited. When stretching is performed by a batch method, the film may be stretched in the stretching direction by gripping the edges of the film.

[0061] When the film is stretched in the MD direction while being continuously transported, for example, a roll longitudinal stretching machine can be used to stretch the film in the MD direction by varying the rotation speed of the rolls transporting the film. In this case, the stretching ratio in the MD direction can be determined by the ratio of the rotation speed of the rolls after stretching to the rotation speed of the rolls before stretching.

[0062] When stretching a film in the TD direction while continuously transporting it, the film can be stretched in the TD direction by clamping both widthwise ends of the film using a transverse stretching machine such as a clip-type tenter and pulling it in the TD direction. In this case, the stretching ratio in the TD direction can be determined by the ratio of the distance between both widthwise ends of the clamped film after stretching to the distance between both widthwise ends of the clamped film before stretching.

[0063] The stretching ratio achieved in the step of stretching the formed film in a specific direction is not particularly limited, but is preferably 1.1 times or more, more preferably 1.3 times or more, even more preferably 1.5 times or more, and particularly preferably 2 times or more. The upper limit is not particularly limited and may be determined appropriately, but may be, for example, 8 times or less, 7 times or less, 5 times or less, or 3 times or less. When biaxial stretching is performed, the above stretching ratio can be adopted for each of the MD direction and the TD direction.

[0064] The stretching temperature is not particularly limited as long as the film can be stretched appropriately, and may be changed depending on the mechanical strength, surface properties, thickness accuracy, etc. required for the stretched film to be produced.

[0065] The stretching temperature is preferably 40°C or higher, more preferably 50°C or higher, and even more preferably 60°C or higher. The upper limit is sufficient as long as it is equal to or lower than the melting point of the poly(3-hydroxybutyrate) resin, and is preferably 150°C or lower, more preferably 145°C or lower, and even more preferably 140°C or lower. When the stretching temperature is within the above temperature range, thickness unevenness of the resulting stretched film can be reduced, and further, mechanical properties such as elongation, tear propagation strength, and flexural fatigue resistance can be improved. Furthermore, problems such as the film sticking to the roll can be prevented.

[0066] The stretching temperature here refers to the temperature of the film during stretching. The stretching temperature can generally be measured by measuring the temperature of the film itself or the ambient temperature near the film using an infrared thermometer, thermolabel, thermocouple, etc.

[0067] The means for adjusting the film temperature during stretching is not particularly limited, and examples thereof include non-contact heating methods such as a method of applying hot air heated to within the above temperature range to the film during stretching, a method of heating the film during stretching using an auxiliary heating means such as an infrared heater, and a method of stretching the film in a heating furnace whose temperature is adjusted to within the above temperature range; and contact heating methods such as a method of bringing the film into contact with a roll heated to within the above temperature range. These methods may be used alone or in combination.

[0068] In the method of bringing the film into contact with rolls heated to within the above temperature range, hot air may be applied to the film between the upstream stretching roll and the downstream stretching roll in the MD direction.

[0069] From the viewpoint of heating efficiency, it is preferable to use a floating heating method as a method for applying hot air heated to within the above temperature range to the film during stretching. Floating heating is a method in which hot air is blown onto both sides of the film from upper and lower nozzles. Multiple upper nozzles and multiple lower nozzles are arranged alternately toward the film surface, and the film can be heated by the hot air blown from each of the upper and lower nozzles without the film coming into contact with either the upper or lower nozzle.

[0070] In the method of using an auxiliary heating means such as an infrared heater to heat the film during stretching, the temperature of the film surface and inside can be raised to the same temperature in a short period of time, enabling uniform stretching throughout the entire film.

[0071] The infrared rays to be irradiated can be electromagnetic waves in the general infrared region, and may be any of near infrared rays: wavelength 0.74 μm to 1.5 μm, mid infrared rays: wavelength 1.5 μm to 3.0 μm, and far infrared rays: wavelength 3.0 μm to 1 mm.

[0072] In the method of bringing the film into contact with rolls heated to the above temperature range, when the film is stretched using two adjacent stretching rolls while being continuously transported, the upstream stretching roll of the two adjacent stretching rolls may be heated to the above temperature range. In this case, the stretching temperature, i.e., the film temperature during stretching, can be controlled by setting the roll temperature to the desired stretching temperature.

[0073] In the process of stretching a molded film in a specific direction, when a strip-shaped film is biaxially stretched, the productivity is excellent and heating can be easily performed, particularly in mass production. Therefore, the order of stretching is to stretch in the MD direction and then in the TD direction. Furthermore, as a means for adjusting the film temperature during stretching, it is preferable to use a method in which the film is brought into contact with a roll heated to within the above temperature range when stretching in the MD direction, and a non-contact heating method in which a heating tool heated to within the above temperature range does not come into contact with the film when stretching in the TD direction.

[0074] (Heat Treatment Step) The heat treatment step of the stretched film is a treatment in which the stretched film is heated by a non-contact heating method to a temperature of (melting point of poly(3-hydroxybutyrate) resin - 40) ° C. or higher and (melting point of poly(3-hydroxybutyrate) resin) ° C. or lower, with a relaxation amount of 9 to 50% in the specific direction, as represented by the following formula (i): Relaxation amount [%] = {(film dimension in specific direction before heat treatment) - (film dimension in specific direction during heat treatment)} / (film dimension in specific direction before heat treatment) × 100 (i)

[0075] In the heat treatment step, the stretched film is heated in a specific direction by a specific relaxation amount. The relaxation in the specific direction refers to relaxation in the stretching direction. Immediately after stretching in the specific direction, the crystal orientation in the specific direction is strong, and a stretched film produced without the heat treatment step of the present disclosure has particularly large heat shrinkage in the specific direction, whereas a stretched film produced through the heat treatment step of the present disclosure has sufficiently small heat shrinkage in the specific direction.

[0076] Here, relaxation refers to reducing the dimensions of a stretched film in a specific direction in order to remove stress in the stretching direction present in the film. Furthermore, the film dimensions refer to the distance between two arbitrarily specified points in the film plane, and may be the distance from one end of the film to the other. When the stretched film of the present disclosure is a strip-shaped film, the film dimensions in the MD direction may be the distance between two arbitrarily specified points in the MD direction in the film plane, and the film dimensions in the TD direction may be the distance between both ends of the film in the width direction. When slack occurs in the film during heat treatment as described below, the film dimensions are the linear distance between two arbitrarily specified points in the film plane, and may be the linear distance from one end of the film to the other end. In particular, the film dimensions in the TD direction may be the linear distance between both ends of the film in the width direction.

[0077] When the film is relaxed using two adjacent rolls while being continuously transported, the film dimension in the MD direction can be adjusted by varying the rotation speed of the two adjacent rolls, while the film dimension in the TD direction can be adjusted by clamping both widthwise ends of the film using a transverse stretching machine such as a clip-type tenter and changing the distance between the clamps.

[0078] Specifically, in the heat treatment step, the amount of relaxation in the MD direction [%] can be calculated by the following formula (i-i), and the amount of relaxation in the TD direction [%] can be calculated by the following formula (i-ii): Amount of relaxation in the MD direction [%] = {(Rotational speed of the upstream roll of two adjacent rolls) - (Rotational speed of the downstream roll of two adjacent rolls)} / (Rotational speed of the upstream roll of two adjacent rolls) x 100 (i-i) Amount of relaxation in the TD direction [%] = {(Distance between both end points in the width direction of the film before heat treatment) - (Distance between both end points in the width direction of the film during heat treatment)} / (Distance between both end points in the width direction of the film before heat treatment) x 100 (i-ii)

[0079] In the stretching step, when biaxial stretching is performed, it is preferable to relax the film in either the MD direction or the TD direction, whichever direction was last stretched. Specifically, for example, when a film is stretched in the MD direction and then stretched in the TD direction, since the crystal orientation in the TD direction is strong after stretching in the TD direction, a stretched film containing a poly(3-hydroxybutyrate)-based resin with little heat shrinkage in either the MD direction or the TD direction can be obtained by heating the film in a specific temperature range with a specific relaxation amount in the TD direction.

[0080] The amount of relaxation in the specific direction may be 9 to 50%, preferably 9 to 40%, more preferably 9 to 30%, and even more preferably 9 to 20%. If the amount of relaxation is less than 9%, the amount of heat shrinkage of the resulting stretched film in the specific direction cannot be sufficiently suppressed, while if it is more than 50%, slack occurs in the film during heat treatment, and not only may slack remain in the resulting stretched film after heat treatment, but the film may also come into contact with a manufacturing apparatus including a heating tool and break, making it impossible to produce a stretched film with good productivity.

[0081] Furthermore, in the manufacturing method of the present disclosure, when a preparatory heat treatment step described below is included, "before heat treatment" in the formula (i) means "before preparatory heat treatment", and "film dimension in a specific direction before heat treatment" in the formula (i) can be read as "film dimension in a specific direction before preparatory heat treatment".

[0082] The heat treatment may be performed two or more times. In this case, it is preferable to increase the amount of relaxation in the specific direction in a stepwise manner. This is because heat shrinkage in the specific direction of the stretched film can be particularly reduced during the stretching process. That is, it is preferable to make the difference between the relaxation amounts in the nth and (n-1)th heat treatments larger than the difference between the relaxation amounts in the (n-1) and (n-2)th heat treatments. Specifically, it is preferable to make the difference between the relaxation amounts in the second and first heat treatments larger than the difference between the relaxation amounts in the first heat treatment, and the difference between the relaxation amounts in the third and second heat treatments larger than the difference between the relaxation amounts in the second and first heat treatments. This can be explained using the following mathematical formula. For example, when the relaxation amount in the specific direction in the nth heat treatment, represented by the formula, is Rn (n is a natural number of 2 or greater), it is preferable that 9%≦Rn≦50%, and when n=2, the following formula (1) is satisfied. When n≧3, it is preferable that the following formula (2) is satisfied throughout the entire range of n from 3 to k (k is a natural number of 3 or greater). R1<R2-R1 (1) R(k-1)-R(k-2)<Rk-R(k-1) (n=k(k≧3)) (2)

[0083] The relaxation amount Rn in the specific direction during the nth heat treatment can be specifically expressed as the following formula (iii): Relaxation amount Rn [%] = {(film dimension in the specific direction before heat treatment) - (film dimension in the specific direction during the nth heat treatment)} / (film dimension in the specific direction before heat treatment) x 100 (iii).

[0084] When the heat treatment is performed at least twice, the first two consecutive times will be particularly described in detail. The heat treatment preferably includes a step of setting the relaxation amount in the specific direction, expressed by the formula, to R1 and then to R2, and the relaxation amounts R1 and R2 preferably satisfy the relationships 9%≦R1≦50%, 9%≦R2≦50%, and R1<R2−R1. Furthermore, it is more preferable that R2 satisfies the relationship 9%≦R2≦30%. By gradually increasing the relaxation amount in the specific direction, heat shrinkage in the specific direction stretched in the film stretching step can be reduced.

[0085] Figure 1 is a diagram explaining the concept of the film relaxation amount, showing an example in which the heat treatment process is performed twice. The solid arrows in Figure 1 indicate the MD direction of the film, the section A-B indicates the process of stretching in the TD direction, the section B-C indicates the first heat treatment process, and the section CD indicates the second heat treatment process. Steps A-D are performed in a continuous process. W1 indicates the film dimension in a specific direction before heat treatment (after stretching in Figure 1), W2 indicates the film dimension during the first heat treatment, and W3 indicates the film dimension during the second heat treatment. The relaxation amount R1 [%] during the first heat treatment can be calculated by (W1-W2) / W1 x 100, and the relaxation amount R2 [%] during the second heat treatment can be calculated by (W1-W3) / W1 x 100.

[0086] The means for heating the film in the heat treatment is not particularly limited as long as it is a non-contact heating method. Examples include a method of applying hot air heated to the temperature range described above to the film, a method of heating the film using an auxiliary heating means such as an infrared heater, and a method of heating the film by placing it in a heating furnace whose temperature is adjusted to the temperature range described above. These methods may be used alone or in combination. Non-contact heating methods make it easy to raise the film temperature, easily adjust the temperature range to between (the melting point of the poly(3-hydroxybutyrate)-based resin - 40) °C and (the melting point of the poly(3-hydroxybutyrate)-based resin) °C, and also avoid the problem of the film sticking to the heating tool.

[0087] The method of applying hot air heated to within the above temperature range to the film, i.e., hot air heating, is a method of applying hot air heated to a temperature range of (melting point of poly(3-hydroxybutyrate)-based resin - 40)°C or more and (melting point of poly(3-hydroxybutyrate)-based resin)°C or less to the film, and a floating type heating method is preferably used.

[0088] The method of heating the film using an infrared heater, that is, infrared radiation heating, is a method of heating the film to the temperature range using an infrared heater, and the infrared rays to be irradiated can be the same as those used when stretching the film.

[0089] In the heat treatment step, the stretched film is heated to a temperature of (melting point of poly(3-hydroxybutyrate)-based resin - 40)°C or more and (melting point of poly(3-hydroxybutyrate)-based resin)°C or less. If the temperature is lower than (melting point of poly(3-hydroxybutyrate)-based resin - 40)°C, the amount of heat shrinkage of the resulting stretched film in the specific direction increases, whereas if the temperature is higher than (melting point of poly(3-hydroxybutyrate)-based resin)°C, the orientation of the crystals obtained by stretching is lost, and the mechanical strength of the resulting stretched film may decrease or the stretched film may melt and break.

[0090] The film temperature in the heat treatment step is preferably (melting point of poly(3-hydroxybutyrate) resin - 40)°C or higher and (melting point of poly(3-hydroxybutyrate) resin)°C or lower, more preferably (melting point of poly(3-hydroxybutyrate) resin - 40)°C or higher and (melting point of poly(3-hydroxybutyrate) resin - 10)°C or lower, and even more preferably (melting point of poly(3-hydroxybutyrate) resin - 40)°C or higher and (melting point of poly(3-hydroxybutyrate) resin - 20)°C or lower. This particularly reduces the risk of film breakage due to melting of the resin.

[0091] The film temperature in the heat treatment step is preferably (melting point of poly(3-hydroxybutyrate) resin - 40)°C or more and (melting point of poly(3-hydroxybutyrate) resin)°C or less, more preferably (melting point of poly(3-hydroxybutyrate) resin - 30)°C or more and (melting point of poly(3-hydroxybutyrate) resin)°C or less, and even more preferably (melting point of poly(3-hydroxybutyrate) resin - 20)°C or more and (melting point of poly(3-hydroxybutyrate) resin)°C or less. This makes it possible to further reduce heat shrinkage in the specific direction of stretching in the film stretching step.

[0092] It is preferable that the heat treatment includes a process of raising the film to temperature T1 and then to temperature T2, and the temperatures T1 and T2 satisfy the condition of the following formula. It is also particularly preferable to include a step of raising the amount of relaxation in the specific direction represented by the formula to R1 and then to R2, and to raise the film to temperature T1 at the relaxation amount R1 and to raise the film to temperature T2 at the relaxation amount R2 under the conditions that the relaxation amounts R1 and R2 satisfy 9%≦R1≦50%, 9%≦R2≦50%, and R1<R2−R1. (melting point of poly(3-hydroxybutyrate)-based resin−40)°C≦T1<T2≦(melting point of poly(3-hydroxybutyrate)-based resin)°C or less

[0093] By gradually increasing the heat treatment temperature, film shrinkage due to rapid crystallization can be suppressed, further reducing the risk of film breakage.

[0094] The melting point of a poly(3-hydroxybutyrate) resin refers to the apex temperature of the melting point peak in a DSC curve obtained by differential scanning calorimetry. Details of differential scanning calorimetry will be described in the Examples section.

[0095] The heating time in the heat treatment step is not particularly limited, but is preferably 1 to 180 seconds, more preferably 1 to 30 seconds, and even more preferably 1 to 10 seconds, from the viewpoint of productivity.

[0096] (Preliminary Heat Treatment Step) A preliminary heat treatment step may be included before the heat treatment step. The preliminary heat treatment refers to a treatment in which the stretched film is heated by a non-contact heating method at a temperature of (melting point of poly(3-hydroxybutyrate)-based resin - 40)°C or higher and (melting point of poly(3-hydroxybutyrate)-based resin)°C or lower, with a relaxation amount in the specific direction of 0% or higher but lower than 9% as represented by the following formula (ii). By including the preliminary heat treatment step, heat shrinkage in the specific direction stretched in the film stretching step can be particularly reduced. Furthermore, the risk of film breakage can be further reduced. Relaxation amount [%] = {(film dimension in specific direction before preliminary heat treatment) - (film dimension in specific direction during preliminary heat treatment)} / (film dimension in specific direction before preliminary heat treatment) × 100 (ii)

[0097] Specifically, in the preliminary heat treatment step, the amount of relaxation in the MD direction [%] can be calculated by the following formula (ii-i), and the amount of relaxation in the TD direction [%] can be calculated by the following formula (ii-ii). Amount of relaxation in the MD direction [%] = {(Rotational speed of the upstream roll of two adjacent rolls) - (Rotational speed of the downstream roll of two adjacent rolls)} / (Rotational speed of the upstream roll of two adjacent rolls) x 100 (ii-i) Amount of relaxation in the TD direction [%] = {(Distance between both end points in the width direction of the film before preliminary heat treatment) - (Distance between both end points in the width direction of the film during preliminary heat treatment)} / (Distance between both end points in the width direction of the film before preliminary heat treatment) x 100 (ii-ii)

[0098] The amount of relaxation in the specific direction represented by formula (ii) in the preliminary heat treatment may be 0% or more and less than 9%, but is preferably 5% or less, more preferably 3% or less, even more preferably 1% or less, and most preferably 0%.

[0099] The means for heating the film in the preliminary heat treatment is not particularly limited as long as it is a non-contact heating method, and may be the same as the means for heating the film in the heat treatment.

[0100] The preferred ranges of the film temperature and heating time in the preliminary heat treatment are the same as the preferred ranges of the film temperature and heating time in the heat treatment step.

[0101] When the stretched film produced by the production method of the present disclosure is heated at 110°C for 10 minutes, the heat shrinkage in the stretching direction is preferably less than 10%, more preferably 8% or less, and even more preferably 6% or less. The smaller the heat shrinkage, the better, but it may be 0% or more, or 1% or more. Details of the method for measuring the heat shrinkage are as described in the Examples section.

[0102] The manufacturing method of the present disclosure may include a step of cooling the film after the step of heat-treating the film. The film temperature in the step of cooling the film may be 100°C or lower, and preferably 50°C or higher and 90°C or lower. As long as the film temperature can be lowered to a temperature lower than the heat treatment temperature, there are no particular limitations on the means for doing so, and examples include a method using the non-contact heating method in which the temperature is controlled to 100°C or lower, preferably 50°C or higher and 90°C or lower. Including the step of cooling the film can prevent a sudden drop in film temperature and the resulting occurrence of wrinkles due to sudden film shrinkage.

[0103] In the production method of the present disclosure, from the viewpoint of productivity, it is preferable to carry out the steps from melting the film raw material in an extruder and then forming it into a film to heat-treating it, particularly up to obtaining a stretched film, as a continuous process. Here, the continuous process refers to obtaining a stretched film by sequentially carrying out the steps from melting the film raw material in an extruder and then forming it into a film, stretching the formed film, heat-treating the stretched film, and, if necessary, cooling the film.

[0104] <Thickness of stretched film> The thickness of the stretched film is not particularly limited and may be appropriately set to the desired thickness. From the viewpoints of uniform thickness, appearance, strength, lightness, etc. of the film, the thickness is preferably 10 to 200 μm, more preferably 15 to 150 μm, and even more preferably 20 to 100 μm. The thickness of the film can be measured using a vernier caliper.

[0105] The stretched film of the present disclosure is thin yet has high strength, and therefore can be suitably used as a packaging film, for example, a packaging film for food and the like that requires heat sealability.

[0106] The following items list preferred aspects of the present disclosure, but the present invention is not limited to them. [Item 1] A method for producing a stretched film containing a poly(3-hydroxybutyrate)-based resin, comprising the steps of melting a film raw material containing the poly(3-hydroxybutyrate)-based resin in an extruder and then forming it into a film, stretching the formed film in a specific direction, and heat-treating the stretched film, wherein the heat treatment is a treatment of heating the stretched film by a non-contact heating method from (the melting point of the poly(3-hydroxybutyrate)-based resin - 40)°C to (the melting point of the poly(3-hydroxybutyrate)-based resin)°C, with a relaxation amount in the specific direction of 9 to 50%, as represented by the following formula (i): Relaxation amount [%] = {(Film dimension in the specific direction before heat treatment) - (Film dimension in the specific direction during heat treatment)} / (Film dimension in the specific direction before heat treatment) × 100 (i) [Item 2] The manufacturing method according to item 1, wherein the heating time in the heat treatment step is 1 to 180 seconds. [Item 3] The manufacturing method according to item 1 or 2, wherein the non-contact heating method is hot air heating or infrared radiation heating. [Item 4] The manufacturing method according to any one of items 1 to 3, wherein the stretching is biaxial stretching. [Item 5] The manufacturing method according to any one of items 1 to 4, wherein the steps from the forming step to the heat treatment are carried out in a continuous process. [Item 6] The manufacturing method according to any one of items 1 to 5, wherein the stretching ratio in the specific direction of the film in the stretching step is 1.1 to 8 times. [Item 7] The manufacturing method according to any one of Items 1 to 6, wherein the poly(3-hydroxybutyrate)-based resin comprises poly(3-hydroxybutyrate-co-3-hydroxyhexanoate). [Item 8] The manufacturing method according to any one of Items 1 to 7, further comprising a pre-heat treatment step prior to the heat treatment step, in which the pre-heat treatment is a treatment in which the stretched film is heated by a non-contact heating method from (the melting point of the poly(3-hydroxybutyrate)-based resin - 40)°C to (the melting point of the poly(3-hydroxybutyrate)-based resin)°C, with a relaxation amount in the specific direction of 0% to less than 9%, as represented by the following formula (ii):Relaxation amount [%] = {(Film dimension in the specific direction before preliminary heat treatment) - (Film dimension in the specific direction during preliminary heat treatment)} / (Film dimension in the specific direction before preliminary heat treatment) × 100 (ii) [Item 9] The manufacturing method according to any one of Items 1 to 8, wherein, in the step of heat treating the stretched film, the heat treatment is performed two or more times, and when the relaxation amount in the specific direction represented by the formula in the nth heat treatment is Rn (n is a natural number of 2 or more), 9% ≦ Rn ≦ 50%, and when n = 2, the following formula (1) is satisfied, and when n ≧ 3, the following formula (2) is satisfied throughout the entire range of n from 3 to k (k is a natural number of 3 or more). R1<R2-R1 (1) R(k-1)-R(k-2)<Rk-R(k-1) (n=k(k≧3)) (2) [Item 10] The manufacturing method according to any one of items 1 to 9, wherein, in the step of heat-treating the stretched film, the heat treatment includes a step of setting the relaxation amount in the specific direction represented by the formula to R1 and then to R2, and the relaxation amounts R1 and R2 satisfy 9%≦R1≦50%, 9%≦R2≦50%, and R1<R2-R1. [Item 11] The manufacturing method according to item 10, wherein, in the step of heat-treating the stretched film, the relaxation amount R2 satisfies 9%≦R2≦30%. [Item 12] The manufacturing method according to any one of items 1 to 11, wherein the heat treatment includes a step of setting the film to a temperature T1 and then to a temperature T2, and the temperatures T1 and T2 satisfy the condition of the following formula: (melting point of poly(3-hydroxybutyrate)-based resin - 40) °C ≦ T1 < T2 ≦ (melting point of poly(3-hydroxybutyrate)-based resin) °C or less [Item 13] The manufacturing method according to Item 12, wherein in the step of heat-treating the stretched film, the heat treatment includes a step of setting the amount of relaxation in the specific direction represented by the formula to R1 and then to R2, wherein the relaxation amounts R1 and R2 satisfy 9% ≦ R1 ≦ 50%, 9% ≦ R2 ≦ 50%, and R1 < R2 - R1, and the film is heated to a temperature T1 at the relaxation amount R1, and the film is heated to a temperature T2 at the relaxation amount R2.

[0107] The present disclosure will be explained in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples in any way.

[0108] The following raw materials were used in the examples and comparative examples. (Poly(3-hydroxybutyrate)-based resin) The poly(3-hydroxybutyrate)-based resins used were poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (P3HB3HH) resins A-1 to A-4 below. In the following, 3HB represents a 3-hydroxybutyrate repeating unit, and 3HH represents a 3-hydroxyhexanoate repeating unit.

[0109] A-1: P3HB3HH (average content ratio 3HB / 3HH = 97.2 / 2.8 (mol% / mol%), glass transition temperature is 6 ° C.) Produced in accordance with the method described in Example 2 of WO 2019 / 142845, and adjusted to a weight average molecular weight of 660,000 g / mol by treatment with an aqueous sodium hydroxide solution. A-2: P3HB3HH (average content ratio 3HB / 3HH = 71.8 / 28.2 (mol% / mol%), glass transition temperature is 1 ° C.) Produced in accordance with the method described in Example 9 of WO 2019 / 142845, and adjusted to a weight average molecular weight of 660,000 g / mol by treatment with an aqueous sodium hydroxide solution. - A-3: P3HB3HH (average content ratio 3HB / 3HH = 94 / 6 (mol% / mol%), glass transition temperature is 6 ° C.) Produced in accordance with the method described in Example 1 of WO 2019 / 142845, and adjusted to a weight average molecular weight of 600,000 g / mol by treatment with an aqueous sodium hydroxide solution. - A-4: P3HB3HH (average content ratio 3HB / 3HH = 94 / 6 (mol% / mol%), glass transition temperature is 6 ° C.) Produced in accordance with the method described in Example 1 of WO 2019 / 142845, and adjusted to a weight average molecular weight of 400,000 g / mol by treatment with an aqueous sodium hydroxide solution. A-5: P3HB3HH (average content ratio 3HB / 3HH=89 / 11 (mol % / mol %), glass transition temperature 6°C) Produced in accordance with the method described in Examples (raw material A-3) of WO 2013 / 147139, and adjusted to a weight average molecular weight of 800,000 g / mol by treatment with an aqueous sodium hydroxide solution.

[0110] (Lubricant) B-1: Behenic acid amide (manufactured by Nippon Fine Chemical Co., Ltd.: BNT-22H)

[0111] (Nucleating Agent) C-1: Pentaerythritol (manufactured by Mitsubishi Chemical Corporation, Neuraizer P)

[0112] (Method for producing resin composition) Resin pellet P-1 Poly(3-hydroxybutyrate)-based resins were used: 30 parts by weight of A-1, 30 parts by weight of A-2, 10 parts by weight of A-3, and 30 parts by weight of A-4, for a total of 100 parts by weight. 0.5 parts by weight of B-1 as a lubricant and 1.0 parts by weight of C-1 as a crystal nucleating agent were dry-blended. The resulting dry blend was placed in a hopper of a φ26 mm co-rotating twin-screw extruder with the cylinder temperature and die temperature set to 150 ° C., melt-kneaded, extruded into strands from the die, passed through a water bath filled with hot water at 45 ° C. to solidify the strands, and cut with a pelletizer to obtain resin pellets P-1. The melting point of the resin pellets P-1 was 153 ° C. The melting point of the poly(3-hydroxybutyrate)-based resin, which is a mixture of A-1 to A-4, was also 153 ° C.

[0113] Resin pellets P-2 Resin pellets P-2 were obtained in the same manner as resin pellets P-1, except that the dry blend was a dry blend of 60 parts by weight of A-3 and 40 parts by weight of A-5 (100 parts by weight in total) as poly(3-hydroxybutyrate)-based resins, and 0.5 parts by weight of B-1 as a lubricant. The melting point of resin pellets P-2 was 143°C. The melting point of the poly(3-hydroxybutyrate)-based resin, which was a mixture of A-3 and A-5, was also 143°C.

[0114] (Weight Average Molecular Weight) The weight average molecular weight of the resin was measured in terms of polystyrene using the aforementioned gel permeation chromatography (HPLC GPC system manufactured by Shimadzu Corporation).

[0115] (Glass Transition Temperature) The glass transition temperature (Tg) of the resin was determined by differential scanning calorimetry in accordance with JIS K-7121. Specifically, first, about 5 mg of the sample to be measured was precisely weighed, and the temperature was raised from -20°C to 200°C at a heating rate of 10°C / min using a differential scanning calorimeter (Seiko Instruments Inc., SSC5200), to obtain a DSC curve. Next, in the obtained DSC curve, the baseline before and after the stepwise change due to the glass transition was extended, and a center line equidistant from these two straight lines in the vertical direction was drawn. The temperature at the point where this center line intersects with the curve of the stepwise change due to the glass transition was taken as the glass transition temperature (Tg).

[0116] (Melting Point) The melting point was determined by differential scanning calorimetry in accordance with JIS K-7121. Specifically, first, about 4 to 5 mg of the sample to be measured was precisely weighed, and the sample was heated from 0°C to 180°C at a heating rate of 10°C / min using a differential scanning calorimeter (Seiko Instruments Inc., SSC5200) to obtain a DSC curve. The apex temperature of the melting point peak in the obtained DSC curve was taken as the melting point.

[0117] (Film Thickness) The thickness was measured at 10 points at 10 cm intervals along the TD direction of the film using a vernier caliper, and the arithmetic mean value of the thicknesses at the 10 points was calculated to be the film thickness.

[0118] (Film Heat Shrinkage) The film to be measured was cut into a square measuring 5 cm in the MD direction x 5 cm in the TD direction, and heated for 10 minutes in an oven set to 110°C. Furthermore, the dimensions of the film in the MD direction and the TD direction after heating were measured, and the heat shrinkage in the MD and TD directions was calculated using the following formula. If the heat shrinkage was less than 10%, it was judged as ◯, and if it was 10% or more, it was judged as ×. Heat shrinkage [%] = (1 - (dimension after heating) / (dimension before heating)) x 100

[0119] Example 1 The cylinder temperature and die temperature of a φ40 mm single-screw extruder connected to a 350 mm wide T-die were each set to 165°C. 60 parts by weight of the resin pellets P-1 and 40 parts by weight of polylactic acid (NatureWorks, Ingeo 4060D, melting point 210°C) were dry-blended. The dry-blended product was fed into the single-screw extruder and melted, and the molten resin at a temperature of 165°C was extruded into a film using a T-die. The film-like molten resin was extruded onto a casting roll set at 40°C and molded at a take-up speed of 2 m / min. After cooling to a film temperature of 30°C, the film was peeled off from the casting roll to obtain a film with a thickness of approximately 300 μm.

[0120] The film peeled from the casting roll was taken up by a take-up roll and continuously stretched in the MD direction by a roll longitudinal stretching machine at a film temperature of 60°C during stretching to a stretch ratio of 2.9 times. The film temperature at this time was controlled by adjusting the roll temperature in the roll longitudinal stretching machine to the same temperature (60°C). Subsequently, the film was continuously stretched in the TD direction by a clip-type tenter transverse stretching machine at a film temperature of 70°C during stretching to a stretch ratio of 4.5 times. The film temperature at this time was controlled by applying hot air (air flow) at the same temperature (70°C) to the film in the transverse stretching machine.

[0121] Next, the film was subjected to a heat treatment in a clip-type tenter transverse stretching machine by applying 130°C hot air to the film at a film temperature of 130°C, a heating time of 10 seconds, and a relaxation amount in the TD direction of 10%, to obtain a biaxially stretched film with a thickness of 25 μm. The heat shrinkage of the obtained film at 110°C was measured, and the heat shrinkage was 2% in the MD direction and 7% in the TD direction, which was less than 10%, making it an excellent film. The results are shown in Table 1.

[0122]

[0123] Examples 2 to 5, Comparative Examples 1 to 5 Biaxially stretched films were obtained in the same manner as in Example 1, except that the resin composition, stretch ratio, and heat treatment conditions were changed as shown in Table 1, and the heat shrinkage of the obtained films was measured. The results are shown in Table 1.

[0124] In Examples 1 to 5, in which the heat treatment temperature was 120 to 153°C, which was in the range of (melting point of poly(3-hydroxybutyrate)-based resin -40)°C or higher and the relaxation amount was 10 to 30%, which was in the range of 9 to 50%, excellent biaxially stretched films were obtained, with heat shrinkage amounts in both the MD and TD directions being less than 10%. On the other hand, in Comparative Example 2, since there was no heat treatment step, the heat shrinkage amounts in both the MD and TD directions were 10% or higher. In Comparative Examples 1, 3, and 5, the heat treatment temperature or the relaxation amount during heat treatment was low, so a sufficient heat treatment effect was not obtained, and the heat shrinkage amount in the TD direction was 10% or higher. In Comparative Example 4, the relaxation amount during heat treatment was set to a large value of 60%, so slack occurred in the film after heat treatment. If slack occurs in the film, the film may come into contact with the manufacturing equipment, including the heating equipment, and the film may break.

[0125] Example 6 The cylinder temperature and die temperature of a φ40 mm single-screw extruder connected to a 350 mm wide T-die were each set to 165 ° C. 80 parts by weight of the resin pellets P-2 and 20 parts by weight of polylactic acid (Total Corbion PLA, Luminy LX175, melting point 151 ° C.) were dry-blended. The dry blend was introduced into the single-screw extruder and melted, and the molten resin at a temperature of 165 ° C. was extruded into a film using a T-die. The film-like molten resin was extruded onto a cast roll set at 40 ° C. and molded at a take-up speed of 2 m / min. After cooling to a film temperature of 40 ° C., the film was peeled off from the cast roll to obtain a film with a thickness of approximately 300 μm.

[0126] The film peeled from the casting roll was taken up by a take-up roll and continuously stretched in a roll longitudinal stretching machine so that the film temperature during stretching was 60 ° C. and the stretching ratio in the MD direction was 3 times. The film temperature at this time was controlled by adjusting the roll temperature in the roll longitudinal stretching machine to the same temperature (60 ° C.). The obtained MD-stretched film was cut into MD 90 mm × TD 350 mm and stretched in the TD direction using a uniaxial stretching machine so that the film temperature during stretching was 70 ° C. and the stretching ratio was 5 times. The film temperature at this time was controlled by applying hot air (air flow) at the same temperature (70 ° C.) to the film in the stretching machine.

[0127] Subsequently, the film was subjected to a preliminary heat treatment in a uniaxial stretching machine by applying hot air at 120°C to the film at a film temperature of 120°C for 30 seconds with a relaxation amount in the TD direction of 0%.

[0128] Next, the film was subjected to a heat treatment in a uniaxial stretching machine by applying 120°C hot air to the film at a temperature of 120°C for 30 seconds, with a relaxation amount in the TD direction of 20%, to obtain a biaxially stretched film with a thickness of 25 μm. The heat shrinkage of the obtained film at 110°C was measured, and the heat shrinkage was 2% in the MD direction and 4% in the TD direction, which was less than 10%, making it an excellent film. The results are shown in Table 2.

[0129] <Examples 7 to 10> Biaxially stretched films were obtained in the same manner as in Example 6, except that the presence or absence of preliminary heat treatment or the conditions for preliminary heat treatment, or the conditions for heat treatment, were changed as shown in Table 2, and the heat shrinkage of the obtained films was measured. The results are shown in Table 2.

[0130]

[0131] In Examples 6 to 10, in which the heat treatment temperature was 120 to 130°C, which is in the range of (melting point of poly(3-hydroxybutyrate)-based resin -40)°C or higher and (melting point of poly(3-hydroxybutyrate)-based resin)°C or lower, and the relaxation amount was 10 to 30%, which is in the range of 9 to 50%, excellent biaxially stretched films were obtained in which the heat shrinkage in both the MD and TD directions was less than 10%. Furthermore, by including a pre-heat treatment step as in Examples 6 and 7, or by performing two-stage heat treatment with the relaxation amount gradually increased as in Example 10, it is possible to particularly reduce heat shrinkage in the specific direction stretched in the film stretching step.

Claims

1. A method for producing a stretched film containing a poly(3-hydroxybutyrate)-based resin, comprising the steps of melting a film raw material containing the poly(3-hydroxybutyrate)-based resin in an extruder, and then forming the film into a film, stretching the formed film in a specific direction, and heat-treating the stretched film, wherein the heat treatment is a treatment in which the stretched film is heated by a non-contact heating method from (melting point of poly(3-hydroxybutyrate)-based resin -40)°C to (melting point of poly(3-hydroxybutyrate)-based resin)°C with a relaxation amount of 9 to 50% in the specific direction, as represented by the following formula (i): Relaxation amount [%] = {(film dimension in specific direction before heat treatment) - (film dimension in specific direction during heat treatment)} / (film dimension in specific direction before heat treatment) x 100 (i) 2. The method according to claim 1, wherein the heating time in the heat treatment step is 1 to 180 seconds.

3. The method according to claim 1 or 2, wherein the non-contact heating method is hot air heating or infrared radiation heating.

4. The method according to claim 1 or 2, wherein the stretching is biaxial stretching.

5. The method according to claim 1 or 2, wherein the steps from the molding step to the heat treatment step are carried out in a continuous process.

6. The method according to claim 1 or 2, wherein the stretching ratio of the film in the specific direction in the stretching step is 1.1 to 8 times.

7. The method according to claim 1 or 2, wherein the poly(3-hydroxybutyrate)-based resin comprises poly(3-hydroxybutyrate-co-3-hydroxyhexanoate).

8. The method according to claim 1 or 2, further comprising a step of performing a preliminary heat treatment prior to the heat treatment step, wherein the preliminary heat treatment is a treatment in which the stretched film is heated by a non-contact heating method from (melting point of poly(3-hydroxybutyrate)-based resin -40)°C to (melting point of poly(3-hydroxybutyrate)-based resin)°C with a relaxation amount in the specific direction of 0% or more and less than 9%, as represented by the following formula (ii): Relaxation amount [%] = {(film dimension in the specific direction before preliminary heat treatment) - (film dimension in the specific direction during preliminary heat treatment)} / (film dimension in the specific direction before preliminary heat treatment) x 100 (ii) 9. The method according to claim 1 or 2, wherein in the step of heat-treating the stretched film, the heat treatment includes a step of setting the amount of relaxation in the specific direction represented by the formula to R1 and then to R2, and the amounts of relaxation R1 and R2 satisfy 9%≦R1≦50%, 9%≦R2≦50%, and R1<R2-R1.

10. The method according to claim 9, wherein in the step of heat treating the stretched film, the relaxation amount R2 satisfies 9%≦R2≦30%.

11. The method according to claim 1 or 2, wherein the heat treatment includes a treatment of bringing the film to temperature T1 and then to temperature T2, and the temperatures T1 and T2 satisfy the following formula: (melting point of poly(3-hydroxybutyrate)-based resin - 40) ° C. ≦ T1 < T2 ≦ (melting point of poly(3-hydroxybutyrate)-based resin) ° C. or less.

12. The method of manufacturing according to claim 11, wherein in the step of heat-treating the stretched film, the heat treatment includes a step of setting the amount of relaxation in the specific direction represented by the formula to R1 and then to R2, the relaxation amounts R1 and R2 satisfying 9%≦R1≦50%, 9%≦R2≦50%, and R1<R2-R1, the film is brought to a temperature T1 at the relaxation amount R1, and the film is brought to a temperature T2 at the relaxation amount R2.

Citation Information

Patent Citations

  • polyhydroxy acid film

    JP1993508819A

  • Microorganism-decomposable film

    JP1997132701A

  • Uniaxially stretched aliphatic polyester film and its production

    JP1997314658A

  • High strength film comprising polyhydroxyalkane and manufacturing method therefor

    JP2003311825A

  • Manufacturing method of biaxially oriented film

    JP2022062759A

Cited By

  • Polylactic acid oriented film and preparation method thereof

    CN119592033A

  • Method for producing stretched film

    WO2025182626A1