Composition, cured product and optical member

The combination of benzobisdithiol compounds with anti-fading agents in a curable composition addresses the limitations of existing ultraviolet absorbers by enhancing absorption at 400 nm and light resistance, ensuring stable performance under prolonged light exposure.

WO2024203670A1PCT designated stage expired Publication Date: 2024-10-03FUJIFILM CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010892
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-02-09
Filing Date
2024-03-21
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current ultraviolet absorbers face challenges in maintaining high absorption efficiency for longer wavelengths around 400 nm and suffer from poor light resistance, leading to decreased performance over time, especially when exposed to light irradiation.

Method used

A composition comprising an ultraviolet absorber, a curable compound, and an anti-fading agent, specifically using benzobisdithiol compounds with a specific structure and combining them with amine, phenol, hydroquinone, or benzolactone compounds to enhance absorption and resistance, forming a cured product with improved light stability.

Benefits of technology

The composition achieves excellent ultraviolet absorption at 400 nm with minimal coloration and superior light resistance, maintaining performance even after long-term light exposure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010892_03102024_PF_FP_ABST
    Figure JP2024010892_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed is a composition which contains an ultraviolet absorbent, a curable compound and a color fading inhibitor, wherein: the ultraviolet absorbent contains at least one substance that is selected from among a compound represented by formula (1) and a polymer containing a structure derived from the compound represented by formula (1); and the color fading inhibitor contains at least one compound that is selected from among an amine compound, a phenolic compound, a hydroquinone compound, a catechol compound, an ascorbic acid compound, a carotenoid compound, a metal complex compound, and a benzolactone compound. Also disclosed are a cured product and an optical member, each using the above-described composition.
Need to check novelty before this filing date? Find Prior Art

Description

Composition, cured product, and optical component

[0001] The present invention relates to a composition containing an ultraviolet absorber. The present invention also relates to a cured product and an optical component using a composition containing an ultraviolet absorber.

[0002] Benzobisdithiol compounds have excellent ultraviolet absorption properties and are used as ultraviolet absorbers, etc. For example, Patent Document 1 describes the use of a specific benzobisdithiol as an ultraviolet absorber.

[0003] JP 2009-067984 A

[0004] One of the required properties of ultraviolet absorbers is that they are less colored. In recent years, they have also been required to have a high absorption capacity for ultraviolet rays with longer wavelengths, such as those in the vicinity of 400 nm.

[0005] In addition, the ultraviolet absorption performance of ultraviolet absorbers may decrease over time due to light irradiation. In particular, ultraviolet absorbers whose maximum absorption wavelength is on the longer wavelength side of the ultraviolet region tend to have poor light resistance and tend to have a tendency to easily decrease ultraviolet absorption ability over time. For this reason, in recent years, there has been a demand for further improvement in the light resistance of ultraviolet absorbers.

[0006] Therefore, an object of the present invention is to provide a composition that can be used to produce a cured product that has excellent absorption ability for ultraviolet light with a wavelength of around 400 nm, is less colored, and has excellent light resistance. Another object of the present invention is to provide a cured product and an optical component.

[0007] The present inventors have conducted extensive research into compounds having a skeleton represented by formula (1), and have found that Q 1 and Q 2 It has been found that a compound having a specific combination of the above structures has excellent absorption ability for ultraviolet light having a wavelength of around 400 nm, has little coloring, and is excellent in light resistance. Further investigation has revealed that by using this compound in combination with a predetermined anti-fading agent, a film with little coloring even after long-term light irradiation can be obtained, and this has led to the completion of the present invention. Therefore, the present invention provides the following.

[0008] <1> A composition comprising an ultraviolet absorber, a curable compound, and a discoloration inhibitor, wherein the ultraviolet absorber comprises at least one selected from a compound represented by formula (1) and a polymer containing a structure derived from the compound represented by formula (1), and the discoloration inhibitor comprises at least one selected from an amine compound, a phenol compound, a hydroquinone compound, a catechol compound, an ascorbic acid compound, a carotenoid compound, a metal complex compound, and a benzolactone compound; In formula (1), Q 1 represents a group represented by formula (Q-1); Q 2 is =O, =S, =NR q1 or =CR q2 R q3 represents R q1 ~R q3 each independently represents a hydrogen atom or a substituent, R q2 and R q3 may be bonded to each other to form a ring; provided that R q2 and R q3 When they are bonded to form a ring, =CR q2 R q3 Is Q 1 is not identical in structure to R 1 and R 2 each independently represents a hydrogen atom or a substituent; 1 ~X 4 are each independently —S—, —NR X1 - or -SO 2 represents -, and R X1 represents a hydrogen atom or an alkyl group; In formula (Q-1), * represents a bond, R 101 and R 102 each independently represents a hydrogen atom, an alkyl group, an aralkyl group, an aryl group, a heterocyclic group, or a group containing a polymerizable group having an ethylenically unsaturated bond; 101 or R 102 When either one of R is a hydrogen atom, the other represents an alkyl group, an aralkyl group, an aryl group, a heterocyclic group, or a group containing a polymerizable group having an ethylenically unsaturated bond, 101 or R 102When either one of R is a methyl group, the other represents a hydrogen atom, an alkyl group having two or more carbon atoms, an aralkyl group, an aryl group, a heterocyclic group, or a group containing a polymerizable group having an ethylenically unsaturated bond, 101 or R 102 When either one of the above is a phenyl group, the other represents a hydrogen atom, an alkyl group, an aralkyl group, a substituted aryl group, a heterocyclic group, or a group containing a polymerizable group having an ethylenically unsaturated bond. <2> The composition according to <1>, wherein the compound represented by formula (1) is a compound represented by formula (3): In formula (3), Q 3 represents a group represented by the above formula (Q-1); Q 4 is =O, =S, =NR q11 or =CR q12 R q13 represents R q11 ~R q13 each independently represents a hydrogen atom or a substituent, R q12 and R q13 may be bonded to each other to form a ring; provided that R q12 and R q13 When they are bonded to form a ring, =CR q12 R q13 Is Q 3 is not identical in structure to R 11 and R 12 are each independently —OH, —O—Y 11 , -OC(=O)-Y 11 , -OC(=O)O-Y 11 , -OC(=O)NR y11 -Y 11 , -OSO 2 -Y 11 or a group containing a polymerizable group having an ethylenically unsaturated bond, R y11 represents a hydrogen atom, an alkyl group, an aralkyl group, or an aryl group; Y 11 represents an alkyl group, an aralkyl group, or an aryl group. <3> The composition according to <1> or <2>, wherein the anti-fading agent includes at least one selected from the group consisting of a compound represented by formula (Ao1-1) and a compound represented by formula (Ao2-1). In formula (Ao1-1), R a1 ~Ra4 each independently represents a hydrogen atom, an alkyl group, or an alkenyl group; a1 represents a hydrogen atom, an alkyl group, an alkenyl group, an alkoxy group, an alkenyloxy group, an alkoxycarbonyl group, an alkenyloxycarbonyl group, an aryloxycarbonyl group, an acyl group, an acyloxy group, an alkoxycarbonyloxy group, an alkenyloxycarbonyloxy group, an aryloxycarbonyloxy group, an alkylsulfonyl group, an alkenylsulfonyl group, an arylsulfonyl group, an alkylsulfinyl group, an alkenylsulfinyl group, an arylsulfinyl group, a sulfamoyl group, a carbamoyl group, a hydroxy group or an oxy radical group; X a2 represents an atomic group necessary to form a 5- to 7-membered ring; p1 represents a hydrogen atom, an alkyl group, an alkenyl group, an aryl group, a heterocyclic group, an acyl group, an alkoxycarbonyl group, an alkenyloxycarbonyl group, an aryloxycarbonyl group, an alkylsulfonyl group, an arylsulfonyl group, or —Si(R p101 ) (R p102 ) (R p103 ) and R p101 ~R p103 each independently represents an alkyl group, an alkenyl group, an aryl group, an alkoxy group, an alkenyloxy group, or an aryloxy group; R p2 ~R p6 each independently represents a hydrogen atom or a substituent, p1 ~R p6 two adjacent groups among R may be bonded to form a ring; p1 ~R p6 <4> The composition according to <1> or <2>, wherein the anti-fading agent includes at least one selected from the group consisting of a compound represented by formula (Ao1-2) and a compound represented by formula (Ao2-2): In formula (Ao1-2), X a11represents a hydrogen atom, an alkyl group, an alkenyl group, an alkoxy group, an alkenyloxy group, an alkoxycarbonyl group, an alkenyloxycarbonyl group, an aryloxycarbonyl group, an acyl group, an acyloxy group, an alkoxycarbonyloxy group, an alkenyloxycarbonyloxy group, an aryloxycarbonyloxy group, an alkylsulfonyl group, an alkenylsulfonyl group, an arylsulfonyl group, an alkylsulfinyl group, an alkenylsulfinyl group, an arylsulfinyl group, a sulfamoyl group, a carbamoyl group, a hydroxy group, or an oxy radical group; R a11 represents a substituent; in formula (Ao2-2), R p11 ~R p14 each independently represents a hydrogen atom, an alkyl group, or an alkenyl group; Y p11 represents an aryl group, a heteroaryl group, or an ethylenically unsaturated bond-containing group. <5> The composition according to any one of <1> to <4>, wherein the curable compound includes at least one selected from a resin and a polymerizable compound. <6> The composition according to any one of <1> to <4>, wherein the curable compound includes a resin, and the resin is at least one selected from a (meth)acrylic resin, a polystyrene resin, a polyester resin, a polyurethane resin, a thiourethane resin, a polyimide resin, an epoxy resin, a polycarbonate resin, a phthalate resin, a cellulose acylate resin, and a cyclic olefin resin. <7> A cured product obtained using the composition according to any one of <1> to <6>. <8> An optical member including the cured product according to <7>.

[0009] According to the present invention, it is possible to provide a composition that can be used to produce a cured product that has excellent absorption ability for ultraviolet light with a wavelength of around 400 nm, is less colored, and has excellent light resistance.The present invention also provides a cured product and an optical component.

[0010] The present invention will be described in detail below. In the present specification, when a group (atomic group) is represented without specifying whether it is substituted or unsubstituted, it encompasses both unsubstituted and substituted groups. For example, the term "alkyl group" encompasses not only unsubstituted alkyl groups (unsubstituted alkyl groups) but also substituted alkyl groups (substituted alkyl groups). In the present specification, a numerical range expressed using "to" refers to a range that includes the numerical values ​​before and after "to" as the lower and upper limits. In the present specification, the term "total solids" refers to the total amount of all components of a resin composition excluding the solvent. In the present specification, "(meth)acrylate" refers to either or both of acrylate and methacrylate, "(meth)acrylic" refers to either or both of acrylic and methacrylic, "(meth)allyl" refers to either or both of allyl and methallyl, and "(meth)acryloyl" refers to either or both of acryloyl and methacryloyl. In this specification, the term "process" does not only mean an independent process, but also includes a process that cannot be clearly distinguished from other processes as long as the intended effect of the process is achieved. In this specification, the weight average molecular weight (Mw) and number average molecular weight (Mn) are defined as values ​​measured by gel permeation chromatography (GPC) in terms of polystyrene.

[0011] <Composition> The composition of the present invention comprises an ultraviolet absorber, a curable compound, and a discoloration inhibitor, wherein the ultraviolet absorber comprises at least one selected from the group consisting of a compound represented by formula (1) and a polymer containing a structure derived from the compound represented by formula (1), and the discoloration inhibitor comprises at least one selected from the group consisting of an amine compound, a phenol compound, a hydroquinone compound, a catechol compound, an ascorbic acid compound, and a benzolactone compound.

[0012] The compound represented by formula (1) and the polymer containing a structure derived from the compound represented by formula (1) are compounds with excellent absorption of ultraviolet light with a wavelength of around 400 nm, little coloration, and excellent light resistance, such as resistance to decomposition due to light irradiation. The composition of the present invention, which contains at least one ultraviolet absorber selected from the compound represented by formula (1) and the polymer containing a structure derived from the compound represented by formula (1), can produce cured products with excellent absorption of ultraviolet light with a wavelength of around 400 nm, little coloration, and excellent light resistance. The composition of the present invention further contains at least one anti-fading agent selected from amine compounds, phenolic compounds, hydroquinone compounds, catechol compounds, ascorbic acid compounds, and benzolactone compounds, thereby suppressing decomposition of the compound represented by formula (1) or the polymer containing a structure derived from the compound represented by formula (1), even after long-term light irradiation of a film obtained using the composition. Therefore, the composition of the present invention can produce a film with little coloration even after long-term light irradiation. Therefore, the composition of the present invention can produce cured products with excellent absorption of ultraviolet light with a wavelength of around 400 nm, little coloration, and excellent light resistance.

[0013] The composition of the present invention may be a composition in the form of a solution containing a solvent. The composition of the present invention may also be a kneaded product. In this specification, the kneaded product refers to a product obtained by kneading a resin with an ultraviolet absorber containing at least one selected from the group consisting of a compound represented by formula (1) and a polymer containing a structure derived from the compound represented by formula (1). That is, the kneaded product referred to in this specification refers to a product in which an ultraviolet absorber is mixed and dispersed in a resin, and is different from a solution in which an ultraviolet absorber and a resin are dissolved or dispersed in a solvent. When the composition of the present invention is a kneaded product, a curable compound containing a resin is used.

[0014] The kneaded material is preferably in the form of pellets. In this specification, pellets refer to a material obtained by granulating (pelletizing) the kneaded material into a fixed shape such as a sphere, ellipsoid, cylinder, or prism. The pellets are also preferably master pellets (master batches). Master pellets (master batches) refer to a material in which a high concentration of additives such as an ultraviolet absorber is dispersed in a resin, and are mixed with a resin or the like at a specified ratio when forming a molded body.

[0015] Each component contained in the composition of the present invention will be described below.

[0016] <<Ultraviolet Absorber>> The composition of the present invention contains an ultraviolet absorber. The ultraviolet absorber used contains at least one selected from a compound represented by formula (1) and a polymer containing a structure derived from the compound represented by formula (1). The ultraviolet absorber preferably contains a compound represented by formula (1). Hereinafter, the compound represented by formula (1) will also be referred to as a specific compound. Furthermore, a polymer containing a structure derived from the compound represented by formula (1) will also be referred to as a specific polymer. Furthermore, the specific compound and the specific polymer will collectively be referred to as a specific ultraviolet absorber.

[0017] <<<<Specific Ultraviolet Absorber>>> (Compound Represented by Formula (1) (Specific Compound)) First, the compound represented by Formula (1) (specific compound) will be described. In formula (1), Q 1 represents a group represented by formula (Q-1); Q 2 is =O, =S, =NR q1 or =CR q2 R q3 represents R q1 ~R q3 each independently represents a hydrogen atom or a substituent, R q2 and R q3 may be bonded to each other to form a ring; provided that R q2 and R q3 When they are bonded to form a ring, =CR q2 R q3 Is Q 1 is not identical in structure to R 1 and R 2each independently represents a hydrogen atom or a substituent; 1 ~X 4 are each independently —S—, —NR X1 - or -SO 2 represents -, and R X1 represents a hydrogen atom or an alkyl group; In formula (Q-1), * represents a bond, R 101 and R 102 each independently represents a hydrogen atom, an alkyl group, an aralkyl group, an aryl group, a heterocyclic group, or a group containing a polymerizable group having an ethylenically unsaturated bond; 101 or R 102 When either one of R is a hydrogen atom, the other represents an alkyl group, an aralkyl group, an aryl group, a heterocyclic group, or a group containing a polymerizable group having an ethylenically unsaturated bond, 101 or R 102 When either one of R is a methyl group, the other represents a hydrogen atom, an alkyl group having two or more carbon atoms, an aralkyl group, an aryl group, a heterocyclic group, or a group containing a polymerizable group having an ethylenically unsaturated bond, 101 or R 102 When one of the groups is a phenyl group, the other represents a hydrogen atom, an alkyl group, an aralkyl group, a substituted aryl group, a heterocyclic group, or a group containing a polymerizable group having an ethylenically unsaturated bond.

[0018] -R 1 , R 2 Regarding - R in formula (1) 1 and R 2 The substituent represented by is an alkyl group, an aryl group, an aralkyl group, a heterocyclic group, a group containing a polymerizable group having an ethylenically unsaturated bond, —OH, —O—Y 11 , -OC(=O)-Y 11 , -OC(=O)O-Y 11 , -OC(=O)NR y11 -Y 11 , -OSO 2 -Y 11 , a cyano group, a halogen atom, and a nitro group. y11 represents a hydrogen atom, an alkyl group, an aralkyl group, or an aryl group; Y 11represents an alkyl group, an aralkyl group, or an aryl group.

[0019] The number of carbon atoms in the alkyl group is preferably 1 to 30, more preferably 1 to 20, even more preferably 1 to 15, particularly preferably 1 to 10, and most preferably 1 to 8. The alkyl group may be linear, branched, or cyclic, and is preferably linear or branched. The alkyl group may have a substituent. Examples of the substituent include the groups described below for the substituent T.

[0020] The number of carbon atoms in the aryl group is preferably 6 to 30, more preferably 6 to 20, still more preferably 6 to 15, particularly preferably 6 to 10, and most preferably 6 to 8. The aryl group may have a substituent. Examples of the substituent include the groups described below for the substituent T.

[0021] The number of carbon atoms in the alkyl portion of the aralkyl group is preferably 1 to 10, more preferably 1 to 5, and even more preferably 1 to 3. The number of carbon atoms in the aryl portion of the aralkyl group is preferably 6 to 30, more preferably 6 to 20, even more preferably 6 to 15, particularly preferably 6 to 10, and most preferably 6 to 8. The aralkyl group may have a substituent. Examples of the substituent include the groups explained in the description of the substituent T below. Specific examples of the aralkyl group include a benzyl group.

[0022] The heterocycle in the heterocyclic group preferably contains a 5- or 6-membered saturated or unsaturated heterocycle. An aliphatic ring, an aromatic ring, or another heterocycle may be condensed with the heterocycle. Heteroatoms constituting the heterocycle include B, N, O, S, Se, and Te, with N, O, and S being preferred. It is preferred that the carbon atoms in the heterocycle have a free valence (monovalent) (the heterocyclic group is bonded via a carbon atom). The number of carbon atoms in the heterocyclic group is preferably 1 to 40, more preferably 1 to 30, and even more preferably 1 to 20. Examples of saturated heterocycles in the heterocyclic group include a pyrrolidine ring, a morpholine ring, a 2-bora-1,3-dioxolane ring, and a 1,3-thiazolidine ring. Examples of the unsaturated heterocyclic ring in the heterocyclic group include an imidazole ring, a thiazole ring, a benzothiazole ring, a benzoxazole ring, a benzotriazole ring, a benzoselenazole ring, a pyridine ring, a pyrimidine ring, and a quinoline ring.

[0023] Examples of the halogen atom include a chlorine atom, a bromine atom, and an iodine atom.

[0024] In the group containing a polymerizable group having an ethylenically unsaturated bond, examples of the polymerizable group having an ethylenically unsaturated bond include a vinyl group, a (meth)allyl group, a (meth)acryloyl group, a (meth)acryloyloxy group, a (meth)acryloylamino group, and a vinylphenyl group, and a (meth)acryloyloxy group and a vinylphenyl group are preferred.

[0025] Examples of the group containing a polymerizable group having an ethylenically unsaturated bond include a group represented by the following formula (T1): *-X T1 -Y T1 -Z T1 ... (T1)

[0026] In formula (T1), X T1 represents a single bond, -O-, -OC(=O)-, -OC(=O)O- or -OC(=O)NRx 1 represents -, and Rx 1 represents a hydrogen atom, an alkyl group, or an aryl group; Y T1 represents a single bond or a divalent linking group; Z T1represents a polymerizable group having an ethylenically unsaturated bond.

[0027] Rx 1 The alkyl group represented by is preferably an alkyl group having 1 to 30 carbon atoms. Specific examples include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, and an n-butyl group. 1 The aryl group represented by is preferably a substituted or unsubstituted aryl group having 6 to 30 carbon atoms. Specific examples include a phenyl group, a p-tolyl group, and a naphthyl group. 1 is preferably a hydrogen atom.

[0028] X T1 is preferably —O—, —OC(═O)— or —OC(═O)NH—, and more preferably —OC(═O)— from the viewpoint of synthesis.

[0029] Y T1 Examples of the divalent linking group represented by include a hydrocarbon group and a group in which two or more hydrocarbon groups are linked via a single bond or a linking group. Examples of the hydrocarbon group include an aliphatic hydrocarbon group and an aromatic hydrocarbon group, with an aliphatic hydrocarbon group being preferred. The aliphatic hydrocarbon group preferably has 1 to 30 carbon atoms, more preferably 1 to 20, and even more preferably 1 to 15. The aliphatic hydrocarbon group may be linear, branched, or cyclic. The cyclic aliphatic hydrocarbon group may be a monocyclic or fused ring. The cyclic aliphatic hydrocarbon group may have a crosslinked structure. The aromatic hydrocarbon group preferably has 6 to 30 carbon atoms, more preferably 6 to 20, and even more preferably 6 to 10. The hydrocarbon group may have a substituent. Examples of the substituent include the substituent T described below. For example, an example of the substituent includes a hydroxy group. Examples of the linking group linking the two or more hydrocarbon groups include -NH-, -S(=O) 2 -, -O-, -C(=O)-, -OC(=O)-, -C(=O)O-, -NHC(=O)- and -C(=O)NH- are mentioned, and -O-, -C(=O)-, -OC(=O)-, -C(=O)O-, -NHC(=O)- or -C(=O)NH- is preferred.

[0030] Z T1Examples of the polymerizable group having an ethylenically unsaturated bond represented by the formula (I) include a vinyl group, an allyl group, a (meth)acryloyl group, a (meth)acryloyloxy group, a (meth)acryloylamino group, and a vinylphenyl group, and a (meth)acryloyloxy group and a vinylphenyl group are preferred.

[0031] Specific examples of the group represented by formula (T1) include the following groups represented by T-1 to T-32: In the following structural formula, Me is a methyl group, and * is a bond.

[0032]

[0033] R in formula (1) 1 and R 2 are each independently —OH, —O—Y 11 , -OC(=O)-Y 11 , -OC(=O)O-Y 11 , -OC(=O)NR y11 -Y 11 , -OSO 2 -Y 11 Alternatively, it is preferably a group containing a polymerizable group having an ethylenically unsaturated bond. 1 and R 2 may be the same group or different groups. 1 and R 2 are each independently —OH, —O—Y 11 , -OC(=O)-Y 11 , -OC(=O)O-Y 11 , -OC(=O)NR y11 -Y 11 , or -OSO 2 -Y 11 In this embodiment, for the reason of excellent stability, R 1 and R 2 are each independently —OC(═O)—Y 11 , -O-Y 11 or —OC(═O)NR y11 -Y 11 It is more preferable that R y11is preferably a hydrogen atom or an alkyl group, and more preferably a hydrogen atom. 11 is preferably an alkyl group, more preferably a linear or branched alkyl group, and even more preferably a branched alkyl group, because of its excellent solubility. 1 and R 2 In one embodiment, at least one of R is a group containing a polymerizable group having an ethylenically unsaturated bond. According to this embodiment, an effect of suppressing bleeding out in the film can be obtained. In another embodiment, R 1 and R 2 One of them is -O-Y 11 The other is -OC(=O)-Y 11 In another embodiment, R 1 and R 2 One of them is -O-Y 11 or -OC(=O)-Y 11 and the other is a group containing a polymerizable group having an ethylenically unsaturated bond.

[0034] -X 1 ~X 4 Regarding - X in formula (1) 1 ~X 4 are each independently —S—, —NR X1 - or -SO 2 represents -, and R X1 represents a hydrogen atom or an alkyl group. X1 The preferred range of the alkyl group represented by is the same as the alkyl group described above. X1 is preferably a hydrogen atom.

[0035] X in formula (1) 1 ~X 4 is preferably —S— because the effects of the present invention are more pronounced.

[0036] -Q 1 Regarding - Q in equation (1) 1 represents a group represented by formula (Q-1). R in formula (Q-1) 101 and R 102each independently represents a hydrogen atom, an alkyl group, an aralkyl group, an aryl group, a heterocyclic group, or a group containing a polymerizable group having an ethylenically unsaturated bond. 101 or R 102 When either of R represents a hydrogen atom, the other represents an alkyl group, an aralkyl group, an aryl group, a heterocyclic group, or a group containing a polymerizable group having an ethylenically unsaturated bond, 101 or R 102 When either of R is a methyl group, the other represents a hydrogen atom, an alkyl group having two or more carbon atoms, an aralkyl group, an aryl group, a heterocyclic group, or a group containing a polymerizable group having an ethylenically unsaturated bond, 101 or R 102 When one of the groups is a phenyl group, the other represents a hydrogen atom, an alkyl group, an aralkyl group, a substituted aryl group, a heterocyclic group, or a group containing a polymerizable group having an ethylenically unsaturated bond.

[0037] R 101 and R 102 The number of carbon atoms in the alkyl group represented by is preferably 1 to 30. The upper limit is preferably 20 or less, more preferably 15 or less, even more preferably 10 or less, and even more preferably 8 or less. The lower limit is preferably 2 or more, more preferably 3 or more. The alkyl group may be linear, branched, or cyclic, and is preferably linear or branched. The alkyl group may have a substituent. Examples of the substituent include the groups described below for the substituent T.

[0038] R 101 and R 102 The number of carbon atoms in the aryl group represented by is preferably 6 to 30, more preferably 6 to 20, still more preferably 6 to 15, particularly preferably 6 to 10, and most preferably 6 to 8. The aryl group may have a substituent. Examples of the substituent include the groups described below for the substituent T.

[0039] R 101 and R 102The number of carbon atoms in the alkyl portion of the aralkyl group represented by is preferably 1 to 10, more preferably 1 to 5, and still more preferably 1 to 3. The number of carbon atoms in the aryl portion of the aralkyl group is preferably 6 to 30, more preferably 6 to 20, still more preferably 6 to 15, particularly preferably 6 to 10, and most preferably 6 to 8. The aralkyl group may have a substituent. Examples of the substituent include the groups described below for the substituent T.

[0040] R 101 and R 102 Examples of the heterocyclic group represented by include the heterocyclic groups described above.

[0041] R 101 and R 102 Examples of the group containing a polymerizable group having an ethylenically unsaturated bond represented by the formula (V1) include a group represented by the formula (V1): V1 -Y V1 -Z V1 ... (V1)

[0042] In formula (V1), X V1 represents a single bond, —O—, —C(═O)—, —C(═O)O—, or —C(═O)NRx 2 represents -, and Rx 2 represents a hydrogen atom, an alkyl group, or an aryl group; Y V1 represents a single bond or a divalent linking group; Z V1 represents a polymerizable group having an ethylenically unsaturated bond.

[0043] Rx 2 The alkyl group and aryl group represented by are Rx of the group represented by formula (T1). 1 The meanings and preferred ranges of Rx are the same as those of the alkyl group and aryl group represented by Rx. 2 is preferably a hydrogen atom.

[0044] X V1 is preferably a single bond or —C(═O)—, and more preferably a single bond.

[0045] Y V1 The divalent linking group represented by formula (T1) is Y T1The preferred ranges are also the same as those described above for the divalent linking group represented by the formula (I).

[0046] Z V1 Examples of the polymerizable group having an ethylenically unsaturated bond represented by the formula (I) include a vinyl group, an allyl group, a (meth)acryloyl group, a (meth)acryloyloxy group, a (meth)acryloylamino group, and a vinylphenyl group, and a (meth)acryloyloxy group and a vinylphenyl group are preferred.

[0047] Specific examples of the group represented by formula (V1) include the following groups represented by V-1 to V-12: * in the following structural formulas represents a bond.

[0048]

[0049] R in formula (Q-1) 101 and R 102 As one embodiment of the present invention, R 101 and R 102 each independently represents a hydrogen atom, an alkyl group, an aralkyl group, an aryl group, or a heterocyclic group; R 101 or R 102 When either of R is a hydrogen atom, the other represents an alkyl group, an aralkyl group, an aryl group, or a heterocyclic group; 101 or R 102 When one of R is a methyl group, the other represents a hydrogen atom, an alkyl group having two or more carbon atoms, an aralkyl group, an aryl group, or a heterocyclic group; 101 or R 102 When one of R in formula (Q-1) is a phenyl group, the other may be a hydrogen atom, an alkyl group, an aralkyl group, a substituted aryl group, or a heterocyclic group. 101 and R 102 are each independently preferably an alkyl group or an aralkyl group, more preferably an aralkyl group. 101 and R 102 When is an alkyl group, R 101 and R 102 Preferably, each of the alkyl groups represented by is independently an alkyl group having 2 or more carbon atoms.

[0050] R in formula (Q-1)101 and R 102 In another embodiment, R in formula (Q-1) 101 and R 102 In one embodiment, at least one of the groups is a group containing a polymerizable group having an ethylenically unsaturated bond. According to this embodiment, the effect of suppressing bleeding out in the film can be obtained.

[0051] -Q 2 Regarding - Q in equation (1) 2 is =O, =S, =NR q1 or =CR q2 R q3 represents R q1 ~R q3 each independently represents a hydrogen atom or a substituent, R q2 and R q3 may be bonded to each other to form a ring. q2 and R q3 When they are bonded to form a ring, =CR q2 R q3 Is Q 1 It is not the same structure as

[0052] R q1 ~R q3 Examples of the substituent represented by include a cyano group, a carbamoyl group, a sulfamoyl group, a nitro group, an acyl group, an alkylsulfonyl group, an arylsulfonyl group, an alkylsulfinyl group, an arylsulfinyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, an alkyl group, an aryl group, a heterocyclic group, and a group containing a polymerizable group having an ethylenically unsaturated bond. These groups may further have a substituent. Examples of the substituent include the groups listed as the substituent T described below.

[0053] The carbamoyl group includes carbamoyl groups having 1 to 10 carbon atoms, preferably carbamoyl groups having 2 to 8 carbon atoms, and more preferably carbamoyl groups having 2 to 5 carbon atoms.

[0054] The sulfamoyl group includes sulfamoyl groups having 0 to 10 carbon atoms, preferably sulfamoyl groups having 2 to 8 carbon atoms, and more preferably sulfamoyl groups having 2 to 5 carbon atoms.

[0055] The acyl group includes an acyl group having 1 to 20 carbon atoms, preferably an acyl group having 1 to 12 carbon atoms, and more preferably an acyl group having 1 to 8 carbon atoms.

[0056] The alkylsulfonyl group includes alkylsulfonyl groups having 1 to 20 carbon atoms, preferably alkylsulfonyl groups having 1 to 10 carbon atoms, and more preferably alkylsulfonyl groups having 1 to 8 carbon atoms.

[0057] The arylsulfonyl group includes an arylsulfonyl group having 6 to 20 carbon atoms, and an arylsulfonyl group having 6 to 10 carbon atoms is preferred.

[0058] The alkylsulfinyl group includes alkylsulfinyl groups having 1 to 20 carbon atoms, preferably alkylsulfinyl groups having 1 to 10 carbon atoms, and more preferably alkylsulfinyl groups having 1 to 8 carbon atoms.

[0059] The arylsulfinyl group includes an arylsulfinyl group having 6 to 20 carbon atoms, and an arylsulfinyl group having 6 to 10 carbon atoms is preferred.

[0060] The alkoxycarbonyl group includes an alkoxycarbonyl group having 2 to 20 carbon atoms, preferably an alkoxycarbonyl group having 2 to 12 carbon atoms, and more preferably an alkoxycarbonyl group having 2 to 8 carbon atoms.

[0061] The aryloxycarbonyl group includes an aryloxycarbonyl group having 6 to 20 carbon atoms, preferably an aryloxycarbonyl group having 6 to 12 carbon atoms, and more preferably an aryloxycarbonyl group having 6 to 8 carbon atoms.

[0062] The alkyl group may be an alkyl group having 1 to 18 carbon atoms, preferably an alkyl group having 1 to 10 carbon atoms, and more preferably an alkyl group having 1 to 5 carbon atoms.

[0063] The aryl group may be an aryl group having 6 to 20 carbon atoms, preferably an aryl group having 6 to 15 carbon atoms, and more preferably an aryl group having 6 to 10 carbon atoms.

[0064] The heterocycle in the heterocyclic group preferably contains a 5- or 6-membered saturated or unsaturated heterocycle. An aliphatic ring, an aromatic ring, or another heterocycle may be condensed with the heterocycle. Heteroatoms constituting the heterocycle include B, N, O, S, Se, and Te, with N, O, and S being preferred. It is preferred that the carbon atoms in the heterocycle have a free valence (monovalent) (the heterocyclic group is bonded at a carbon atom). The number of carbon atoms in the preferred heterocyclic group is 1 to 40, more preferably 1 to 30, and even more preferably 1 to 20.

[0065] Examples of the group containing a polymerizable group having an ethylenically unsaturated bond include a group represented by formula (U1): *-X U1 -Y U1 -Z U1 ... (U1)

[0066] In formula (U1), X U1 represents a single bond, -C(=O)-, -C(=O)O- or -C(=O)NRx 3 represents -, and Rx 3 represents a hydrogen atom, an alkyl group, or an aryl group; Y U1 represents a single bond or a divalent linking group; Z U1 represents a polymerizable group having an ethylenically unsaturated bond.

[0067] Rx 3 The alkyl group and aryl group represented by are Rx of the group represented by formula (T1). 1 The meanings and preferred ranges of Rx are the same as those of the alkyl group and aryl group represented by Rx. 3 is preferably a hydrogen atom.

[0068] X U1 is -C(=O)O- or -C(=O)NRx 3 Preferably, it is -, and from the viewpoint of synthesis, it is more preferably -C(=O)O-.

[0069] Y U1The divalent linking group represented by formula (T1) is Y T1 The preferred ranges are also the same as those described above for the divalent linking group represented by the formula (I).

[0070] Z U1 Examples of the polymerizable group having an ethylenically unsaturated bond represented by the formula (I) include a vinyl group, an allyl group, a (meth)acryloyl group, a (meth)acryloyloxy group, a (meth)acryloylamino group, and a vinylphenyl group, and a (meth)acryloyloxy group and a vinylphenyl group are preferred.

[0071] Specific examples of the group represented by formula (U1) include the groups represented by U-1 to U-11 below. In the following structural formulas, * represents a bond.

[0072]

[0073] Q in formula (1) 2 is used because the effect of the present invention is more pronounced. q2 R q3 It is preferable that R q2 and R q3 At least one of R is preferably an electron-withdrawing group, q2 and R q3 It is more preferable that R is an electron-withdrawing group. q2 and R q3 It is also preferable that at least one of R is a group containing a polymerizable group having an ethylenically unsaturated bond. q2 and R q3 It is also preferred that one of the groups is a group containing a polymerizable group having an ethylenically unsaturated bond, and the other is an electron-withdrawing group.

[0074] Examples of electron-withdrawing groups include substituents with a Hammett's substituent constant σp value of 0.2 or greater. The Hammett's substituent constant σ value will now be explained. Hammett's rule is an empirical rule proposed by L. P. Hammett in 1935 to quantitatively discuss the influence of substituents on the reaction or equilibrium of benzene derivatives, and is now widely recognized as valid. The substituent constants determined by Hammett's rule include σp and σm values, and these values ​​can be found in many general textbooks. For example, detailed information is provided in J. A. Dean, ed., "Lange's Handbook of Chemistry," 12th Edition, 1979 (McGraw-Hill); "Chemical Domain" Special Edition, No. 122, pp. 96-103, 1979 (Nankodo); and Chem. Rev., Vol. 91, pp. 165-195, 1991. In this specification, a substituent having a Hammett's substituent constant σp value of 0.2 or more indicates an electron-withdrawing group. The electron-withdrawing group is preferably a group having a Hammett's substituent constant σp value of 0.25 or more, more preferably a group having a Hammett's substituent constant σp value of 0.3 or more, and even more preferably a group having a Hammett's substituent constant σp value of 0.35 or more.

[0075] Specific examples of groups having a Hammett's substituent constant σp value of 0.2 or more include a cyano group (σp value = 0.66), a carboxy group (-COOH: σp value = 0.45), an alkoxycarbonyl group (-COOMe: σp value = 0.45), an aryloxycarbonyl group (-COOPh: σp value = 0.44), a carbamoyl group (-CONH 2 : σp value = 0.36), alkylcarbonyl group (-COMe: σp value = 0.50), arylcarbonyl group (-COPh: σp value = 0.43), alkylsulfonyl group (-SO 2 Me: σp value = 0.72), and an arylsulfonyl group (—SO 2 Ph: σp value = 0.68). Me represents a methyl group, and Ph represents a phenyl group. The values ​​in parentheses are the σp values ​​of representative substituents, excerpted from Chem. Rev., 1991, Vol. 91, pp. 165-195.

[0076] R q2 and R q3are preferably each independently a hydrogen atom, a cyano group, a carbamoyl group, a sulfamoyl group, an acyl group, an alkylsulfonyl group, an arylsulfonyl group, an alkylsulfinyl group, an arylsulfinyl group, a nitro group, an alkoxycarbonyl group, an aryloxycarbonyl group, or a group containing a polymerizable group having an ethylenically unsaturated bond.

[0077] In one embodiment, R q2 and R q3 are each independently a hydrogen atom, a cyano group, a carbamoyl group, a sulfamoyl group, an acyl group, an alkylsulfonyl group, an arylsulfonyl group, an alkylsulfinyl group, an arylsulfinyl group, a nitro group, an alkoxycarbonyl group, or an aryloxycarbonyl group. q2 and R q3 Preferably, at least one of R is a cyano group, an alkoxycarbonyl group, a nitro group, or an alkylsulfonyl group. q2 and R q3 are each independently a cyano group or an alkoxycarbonyl group. q2 and R q3 In another preferred embodiment, R q2 or R q3 An embodiment in which one of the groups is a cyano group and the other is an alkoxycarbonyl group is exemplified.

[0078] In another embodiment, R q2 and R q3 It is also preferable that at least one of R is a group containing a polymerizable group having an ethylenically unsaturated bond. q2 and R q3 may each independently be a group containing a polymerizable group having an ethylenically unsaturated bond, and R q2 and R q3 One of the groups may be a group containing a polymerizable group having an ethylenically unsaturated bond, and the other may be an electron-withdrawing group.

[0079] In this specification, "R q2 and R q3 When they are bonded to form a ring, =CRq2 R q3 Is Q 1 The phrase "is not the same structure as Rq in formula (Q-1)" refers not only to the case where a ring other than the structure represented by formula (Q-1) is formed, but also to the case where a ring other than the structure represented by formula (Q-1) is formed, but Rq in formula (Q-1) is not the same structure as Rq in formula (Q-1) 1 and Rq 2 The type of 1 This also includes cases where a ring having a structure that is a different type of group from Q is formed. 2 Is Q 1 It is a group with a different structure.

[0080] =CR q2 R q3 R q2 and R q3 When they bond to each other to form a ring, the ring formed is preferably a ring other than the structure represented by formula (Q-1), because this more significantly enhances the effects of the present invention. Examples of rings other than the structure represented by formula (Q-1) include a cyclopropane ring, a cyclobutane ring, a cyclopentane ring, a cyclohexane ring, a cycloheptane ring, a pyrrolidine ring, a tetrahydrofuran ring, a tetrahydrothiophene ring, an oxazoline ring, a thiazoline ring, a pyrroline ring, a pyrazoline ring, an imidazoline ring, an imidazolidine ring, a piperidine ring, a piperazine ring, a pyran ring, and an indandione ring. These rings may have a substituent at any position.

[0081] R in formula (1) 1 , R 2 , Q 1 and Q 2 At least one of R preferably contains a group containing a polymerizable group having an ethylenically unsaturated bond, 1 , R 2 , Q 1 and Q 2 It is more preferable that one or two of Q in formula (1) contain a group containing a polymerizable group having an ethylenically unsaturated bond. 2 Ga = CR q2 R q3 and R 1 , R 2 , R q2 , R q3 , R 101 and R102 It is preferable that at least one of R is a group containing a polymerizable group having an ethylenically unsaturated bond, 1 , R 2 , R q2 , R q3 , R 101 and R 102 It is more preferable that one or two of the groups contain a group containing a polymerizable group having an ethylenically unsaturated bond. The number of polymerizable groups having an ethylenically unsaturated bond contained in formula (1) is preferably 1 to 2.

[0082] The specific compound is preferably a compound represented by formula (3). In formula (3), Q 3 represents a group represented by the above formula (Q-1); Q 4 is =O, =S, =NR q11 or =CR q12 R q13 represents R q11 ~R q13 each independently represents a hydrogen atom or a substituent, R q12 and R q13 may be bonded to each other to form a ring; provided that R q12 and R q13 When they are bonded to form a ring, =CR q12 R q13 Is Q 3 It is not the same structure as 11 and R 12 are each independently —OH, —O—Y 11 , -OC(=O)-Y 11 , -OC(=O)O-Y 11 , -OC(=O)NR y11 -Y 11 , -OSO 2 -Y 11 or a group containing a polymerizable group having an ethylenically unsaturated bond, R y11 represents a hydrogen atom, an alkyl group, an aralkyl group, or an aryl group; Y 11 represents an alkyl group, an aralkyl group, or an aryl group.

[0083] Q in equation (3) 3 and Q 4 is Q in equation (1).1 and Q 2 The same definition and preferred range are also the same. y11 and Y 11 The preferred range of R y11 and Y 11 is synonymous with.

[0084] In one embodiment, R in formula (3) 11 and R 12 are each independently —OH, —O—Y 11 , -OC(=O)-Y 11 , -OC(=O)O-Y 11 , -OC(=O)NR y11 -Y 11 or -OSO 2 -Y 11 In this embodiment, R 11 and R 12 are each independently —OC(═O)—Y 11 , -O-Y 11 or —OC(═O)NR y11 -Y 11 It is preferable that:

[0085] In another embodiment, R 11 and R 12 In another embodiment, at least one of R 11 and R 12 One of them is -O-Y 11 The other is -OC(=O)-Y 11 In another embodiment, R 11 and R 12 One of them is -O-Y 11 or -OC(=O)-Y 11 and the other is a group containing a polymerizable group having an ethylenically unsaturated bond.

[0086] R in formula (3) 11 , R 12 , Q 3 and Q 4 At least one of R preferably contains a group containing a polymerizable group having an ethylenically unsaturated bond,11 , R 12 , Q 3 and Q 4 It is more preferable that one or two of Q in formula (3) contain a group containing a polymerizable group having an ethylenically unsaturated bond. 4 Ga = CR q12 R q13 and R 11 , R 12 , R q12 , R q13 , R 101 and R 102 It is preferable that at least one of R is a group containing a polymerizable group having an ethylenically unsaturated bond, 11 , R 12 , R q12 , R q13 , R 101 and R 102 It is more preferable that one or two of the groups contain a group containing a polymerizable group having an ethylenically unsaturated bond. The number of polymerizable groups having an ethylenically unsaturated bond contained in formula (3) is preferably 1 to 2.

[0087] The specific compound is preferably a compound represented by formula (6). In formula (6), Q 5 represents a group represented by the above formula (Q-1), 6 is =O, =S, =NR q21 or =CR q22 R q23 represents R q21 ~R q23 each independently represents a hydrogen atom or a substituent, R q22 and R q23 may be bonded to each other to form a ring; provided that R q22 and R q23 When they are bonded to form a ring, =CR q22 R q23 Is Q 5 It is not the same structure as 61 and R 62 are each independently -O-Y 61 , -OC(=O)-Y 61 , -OC(=O)O-Y 61 , -OC(=O)NR y61-Y 61 , or -OSO 2 -Y 61 represents R y61 represents a hydrogen atom, an alkyl group, an aralkyl group, or an aryl group; Y 61 represents an alkyl group, an aralkyl group, or an aryl group.

[0088] Q in equation (6) 5 and Q 6 is Q in equation (1). 1 and Q 2 The same definition and preferred range are also applicable. y61 and Y 61 The preferred range of R y11 and Y 11 is synonymous with.

[0089] R in formula (6) 61 and R 62 are each independently —OC(═O)—Y 11 , -O-Y 11 or —OC(═O)NR y11 -Y 11 It is preferable that R in formula (6) is 61 and R 62 may be the same group or different groups.

[0090] (Substituent T) Examples of the substituent T include the following groups: halogen atoms (for example, chlorine atoms, bromine atoms, and iodine atoms); alkyl groups [linear, branched, and cyclic alkyl groups; Specifically, it includes linear or branched alkyl groups (preferably linear or branched alkyl groups having 1 to 30 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, t-butyl, n-octyl, eicosyl, 2-chloroethyl, 2-cyanoethyl, and 2-ethylhexyl), cycloalkyl groups (preferably cycloalkyl groups having 3 to 30 carbon atoms, such as cyclohexyl, cyclopentyl, and 4-n-dodecylcyclohexyl), bicycloalkyl groups (preferably bicycloalkyl groups having 5 to 30 carbon atoms, i.e., monovalent groups obtained by removing one hydrogen atom from a bicycloalkane having 5 to 30 carbon atoms, such as bicyclo[1,2,2]heptan-2-yl and bicyclo[2,2,2]octan-3-yl), and tricyclo structures having more ring structures. The alkyl groups in the substituents described below (such as the alkyl group of an alkylthio group) also represent alkyl groups within this concept. alkenyl groups [linear, branched, and cyclic alkenyl groups. Specifically, these include linear or branched alkenyl groups (preferably linear or branched alkenyl groups having 2 to 30 carbon atoms, such as vinyl, allyl, prenyl, geranyl, and oleyl), cycloalkenyl groups (preferably cycloalkenyl groups having 3 to 30 carbon atoms, i.e., monovalent groups obtained by removing one hydrogen atom from a cycloalkene having 3 to 30 carbon atoms, such as 2-cyclopenten-1-yl and 2-cyclohexen-1-yl), and bicycloalkenyl groups (preferably bicycloalkenyl groups having 5 to 30 carbon atoms, i.e., monovalent groups obtained by removing one hydrogen atom from a bicycloalkene having one double bond, such as bicyclo[2,2,1]hept-2-en-1-yl and bicyclo[2,2,2]oct-2-en-4-yl). an alkynyl group (preferably a linear or branched alkynyl group having 2 to 30 carbon atoms, for example, an ethynyl group or a propargyl group);

[0091] an aryl group (preferably an aryl group having 6 to 30 carbon atoms, for example, a phenyl group, a p-tolyl group, a naphthyl group, a m-chlorophenyl group, or an o-hexadecanoylaminophenyl group); a heterocyclic group (preferably a monovalent group obtained by removing one hydrogen atom from a 5- or 6-membered aromatic or non-aromatic heterocyclic compound, more preferably a 5- or 6-membered aromatic heterocyclic group having 3 to 30 carbon atoms, for example, a 2-furyl group, a 2-thienyl group, a 2-pyrimidinyl group, or a 2-benzothiazolyl group); a cyano group; a hydroxy group; a nitro group; a carboxy group; an alkoxy group (preferably a straight-chain or branched alkoxy group having 1 to 30 carbon atoms, for example, a methoxy group, an ethoxy group, an isopropoxy group, a t-butoxy group, an n-octyloxy group, or a 2-methoxyethoxy group); an aryloxy group (preferably an aryloxy group having 6 to 30 carbon atoms, for example, a phenoxy group, a 2-methylphenoxy group, a 4-t-butylphenoxy group, a 3-nitrophenoxy group, or a 2-tetradecanoylaminophenoxy group); a heterocyclic oxy group (preferably a heterocyclic oxy group having 2 to 30 carbon atoms, for example, a 1-phenyltetrazole-5-oxy group or a 2-tetrahydropyranyloxy group); an acyloxy group (preferably a formyloxy group, an alkylcarbonyloxy group having 2 to 30 carbon atoms, or an arylcarbonyloxy group having 6 to 30 carbon atoms, for example, a formyloxy group, an acetyloxy group, a pivaloyloxy group, a stearoyloxy group, a benzoyloxy group, or a p-methoxyphenylcarbonyloxy group);

[0092] a carbamoyloxy group (preferably a carbamoyloxy group having 1 to 30 carbon atoms, for example, an N,N-dimethylcarbamoyloxy group, an N,N-diethylcarbamoyloxy group, a morpholinocarbonyloxy group, an N,N-di-n-octylaminocarbonyloxy group, or an N-n-octylcarbamoyloxy group); an alkoxycarbonyloxy group (preferably an alkoxycarbonyloxy group having 2 to 30 carbon atoms, for example, a methoxycarbonyloxy group, an ethoxycarbonyloxy group, a t-butoxycarbonyloxy group, or an n-octylcarbonyloxy group); an aryloxycarbonyloxy group (preferably an aryloxycarbonyloxy group having 7 to 30 carbon atoms, for example, a phenoxycarbonyloxy group, a p-methoxyphenoxycarbonyloxy group, or a p-n-hexadecyloxyphenoxycarbonyloxy group); an amino group (preferably, an amino group, an alkylamino group having 1 to 30 carbon atoms, or an anilino group having 6 to 30 carbon atoms, for example, an amino group, a methylamino group, a dimethylamino group, an anilino group, an N-methyl-anilino group, or a diphenylamino group); an acylamino group (preferably, a formylamino group, an alkylcarbonylamino group having 2 to 30 carbon atoms, or an arylcarbonylamino group having 6 to 30 carbon atoms, for example, a formylamino group, an acetylamino group, a pivaloylamino group, a lauroylamino group, a benzoylamino group, or a 3,4,5-tri-n-octyloxyphenylcarbonylamino group);

[0093] an aminocarbonylamino group (preferably an aminocarbonylamino group having 1 to 30 carbon atoms, for example, a carbamoylamino group, an N,N-dimethylaminocarbonylamino group, an N,N-diethylaminocarbonylamino group, or a morpholinocarbonylamino group); an alkoxycarbonylamino group (preferably an alkoxycarbonylamino group having 2 to 30 carbon atoms, for example, a methoxycarbonylamino group, an ethoxycarbonylamino group, a t-butoxycarbonylamino group, an n-octadecyloxycarbonylamino group, or an N-methylmethoxycarbonylamino group); an aryloxycarbonylamino group (preferably an aryloxycarbonylamino group having 7 to 30 carbon atoms, for example, a phenoxycarbonylamino group, a p-chlorophenoxycarbonylamino group, or an m-n-octyloxyphenoxycarbonylamino group); a sulfamoylamino group (preferably a sulfamoylamino group having 0 to 30 carbon atoms, for example, a sulfamoylamino group, an N,N-dimethylaminosulfonylamino group, or an N-n-octylaminosulfonylamino group); an alkyl or arylsulfonylamino group (preferably an alkylsulfonylamino group having 1 to 30 carbon atoms, or an arylsulfonylamino group having 6 to 30 carbon atoms, for example, a methylsulfonylamino group, a butylsulfonylamino group, a phenylsulfonylamino group, a 2,3,5-trichlorophenylsulfonylamino group, or a p-methylphenylsulfonylamino group); a mercapto group; an alkylthio group (preferably an alkylthio group having 1 to 30 carbon atoms, for example, a methylthio group, an ethylthio group, or an n-hexadecylthio group); an arylthio group (preferably an arylthio group having 6 to 30 carbon atoms, for example, a phenylthio group, a p-chlorophenylthio group, or an m-methoxyphenylthio group); a heterocyclic thio group (preferably a heterocyclic thio group having 2 to 30 carbon atoms, for example, a 2-benzothiazolylthio group, a 1-phenyltetrazol-5-ylthio group);

[0094] a sulfamoyl group (preferably a sulfamoyl group having 0 to 30 carbon atoms, for example, an N-ethylsulfamoyl group, an N-(3-dodecyloxypropyl)sulfamoyl group, an N,N-dimethylsulfamoyl group, an N-acetylsulfamoyl group, an N-benzoylsulfamoyl group, or an N-(N'-phenylcarbamoyl)sulfamoyl group); a sulfo group; an alkyl or arylsulfinyl group (preferably an alkylsulfinyl group having 1 to 30 carbon atoms, or an arylsulfinyl group having 6 to 30 carbon atoms, for example, a methylsulfinyl group, an ethylsulfinyl group, a phenylsulfinyl group, or a p-methylphenylsulfinyl group); an alkyl or arylsulfonyl group (preferably an alkylsulfonyl group having 1 to 30 carbon atoms, or an arylsulfonyl group having 6 to 30 carbon atoms, for example, a methylsulfonyl group, an ethylsulfonyl group, a phenylsulfonyl group, or a p-methylphenylsulfonyl group);

[0095] acyl groups (preferably formyl groups, alkylcarbonyl groups having 2 to 30 carbon atoms, arylcarbonyl groups having 7 to 30 carbon atoms, and heterocyclic carbonyl groups having 4 to 30 carbon atoms and bonded to a carbonyl group at a carbon atom, such as acetyl groups, pivaloyl groups, 2-chloroacetyl groups, stearoyl groups, benzoyl groups, p-n-octyloxyphenylcarbonyl groups, 2-pyridylcarbonyl groups, and 2-furylcarbonyl groups); aryloxycarbonyl groups (preferably aryloxycarbonyl groups having 7 to 30 carbon atoms, such as phenoxycarbonyl groups, o-chlorophenoxycarbonyl groups, m-nitrophenoxycarbonyl groups, and p-t-butylphenoxycarbonyl groups); an alkoxycarbonyl group (preferably an alkoxycarbonyl group having 2 to 30 carbon atoms, for example, a methoxycarbonyl group, an ethoxycarbonyl group, a t-butoxycarbonyl group, or an n-octadecyloxycarbonyl group); a carbamoyl group (preferably a carbamoyl group having 1 to 30 carbon atoms, for example, a carbamoyl group, an N-methylcarbamoyl group, an N,N-dimethylcarbamoyl group, an N,N-di-n-octylcarbamoyl group, or an N-(methylsulfonyl)carbamoyl group); an aryl or heterocyclic azo group (preferably an aryl azo group having 6 to 30 carbon atoms, or a heterocyclic azo group having 3 to 30 carbon atoms, for example, a phenylazo group, a p-chlorophenylazo group, or a 5-ethylthio-1,3,4-thiadiazol-2-ylazo group); an imido group (preferably an N-succinimido group, or an N-phthalimido group); a phosphinyl group (preferably a phosphinyl group having 2 to 30 carbon atoms, for example, a dimethylphosphino group, a diphenylphosphino group, or a methylphenoxyphosphinyl group); a phosphinyl group (preferably a phosphinyl group having 2 to 30 carbon atoms, for example, a phosphinyl group, a dioctyloxyphosphinyl group, or a diethoxyphosphinyl group); a phosphinyloxy group (preferably a phosphinyloxy group having 2 to 30 carbon atoms, for example, a diphenoxyphosphinyloxy group, or a dioctyloxyphosphinyloxy group); a phosphinylamino group (preferably a phosphinylamino group having 2 to 30 carbon atoms, for example, a dimethoxyphosphinylamino group, or a dimethylaminophosphinylamino group);

[0096] Of the groups listed above, in groups having a hydrogen atom, one or more hydrogen atoms may be substituted with the above-mentioned substituent T. Examples of such a substituent include an alkylcarbonylaminosulfonyl group, an arylcarbonylaminosulfonyl group, an alkylsulfonylaminocarbonyl group, and an arylsulfonylaminocarbonyl group. Specific examples include a methylsulfonylaminocarbonyl group, a p-methylphenylsulfonylaminocarbonyl group, an acetylaminosulfonyl group, and a benzoylaminosulfonyl group.

[0097] Specific examples of the specific compound include compounds having the following structure: In the structural formula shown below, Et is an ethyl group, and Me is a methyl group. n Bu is a normal butyl group, t Bu is a tert-butyl group and Ph is a phenyl group.

[0098]

[0099] The maximum absorption wavelength of the specific compound is preferably in the wavelength range of 380 to 420 nm, and more preferably in the wavelength range of 390 to 410 nm.

[0100] The specific compound preferably has a ratio of absorbance at a wavelength of 440 nm to absorbance at a wavelength of 400 nm taken as 1, which is less than 0.02.

[0101] The molar absorption coefficient at the maximum absorption wavelength of the specific compound is preferably 80,000 L / mol cm or more, more preferably 85,000 L / mol cm or more, and even more preferably 90,000 L / mol cm or more. Also, the molar absorption coefficient at a wavelength of 400 nm is preferably 30,000 L / mol cm or more, more preferably 40,000 L / mol cm or more, and even more preferably 50,000 L / mol cm or more. Also, the molar absorption coefficient at a wavelength of 440 nm is preferably 1,000 L / mol cm or less, more preferably 800 L / mol cm or less, and even more preferably 600 L / mol cm or less.

[0102] The absorbance, maximum absorption wavelength, and molar absorption coefficient of a specific compound can be determined by dissolving the specific compound in ethyl acetate to prepare a solution, and measuring the spectrum of the solution using a 1 cm quartz cell at room temperature (25° C.) Examples of the measuring device include a spectrophotometer (UV-1800PC, manufactured by Shimadzu Corporation).

[0103] The specific compound can be produced in accordance with the method described in WO 2009 / 022736.

[0104] Among the specific compounds, the compound represented by formula (6) can also be produced by reacting a compound represented by formula (4) with a compound represented by formula (5).

[0105] In formula (4), Q 5 represents a group represented by the above formula (Q-1), 6 is =O, =S, =NR q21 or =CR q22 R q23 represents R q21 ~R q23 each independently represents a hydrogen atom or a substituent, R q22 and R q23 may be bonded to each other to form a ring; provided that R q22 and R q23 When they are bonded to form a ring, =CR q22 R q23 Is Q 5 It is not the same structure as

[0106] In formula (5), E 51 is -COCl, -O(C=O)Cl, -NR e51 (C═O)Cl, —NCO, —Cl, —Br, —I, or —SO 2 R e52 represents R e51 represents a hydrogen atom, an alkyl group, an aralkyl group, or an aryl group; R e52 represents —Cl or an alkoxy group; Y 51 represents an alkyl group, an aralkyl group, or an aryl group.

[0107] Q in equation (4) 5 and Q 6 is Q in equation (6). 5 and Q 6 The same applies to the preferred range.

[0108] Y in formula (5) 51 The number of carbon atoms in the alkyl group represented by is preferably 1 to 30, more preferably 1 to 20, even more preferably 1 to 15, particularly preferably 1 to 10, and most preferably 1 to 8. The alkyl group may be linear, branched, or cyclic, and is preferably linear or branched. The alkyl group may have a substituent. Examples of the substituent include the groups described above for the substituent T. Y in formula (5) 51The number of carbon atoms of the aryl group represented by is preferably 6 to 30, more preferably 6 to 20, even more preferably 6 to 15, particularly preferably 6 to 10, and most preferably 6 to 8. The aryl group may have a substituent. Examples of the substituent include the groups described above for the substituent T. 51 The number of carbon atoms in the alkyl portion of the aralkyl group represented by is preferably 1 to 10, more preferably 1 to 5, and still more preferably 1 to 3. The number of carbon atoms in the aryl portion of the aralkyl group is preferably 6 to 30, more preferably 6 to 20, still more preferably 6 to 15, particularly preferably 6 to 10, and most preferably 6 to 8. The aralkyl group may have a substituent. Examples of the substituent include the groups described above for the substituent T.

[0109] Y in formula (5) 51 is preferably an alkyl group.

[0110] E in formula (5) 51 R in e51 The alkyl group, aralkyl group and aryl group represented by are Y in formula (5). 51 The groups are the same as those described above.

[0111] E in formula (5) 51 R in e52 The alkoxy group represented by the formula (I) preferably has 1 to 30 carbon atoms, more preferably 1 to 20 carbon atoms, even more preferably 1 to 15 carbon atoms, particularly preferably 1 to 10 carbon atoms, and most preferably 1 to 8 carbon atoms.

[0112] The reaction between the compound represented by formula (4) and the compound represented by formula (5) can be carried out in an organic solvent. The organic solvent is not particularly limited, but examples thereof include amide solvents such as dimethylformamide, dimethylacetamide, and N-methyl-2-pyrrolidone, tetrahydrofuran, acetonitrile, toluene, methanol, ethanol, isopropyl alcohol, and mixtures thereof, with dimethylformamide or dimethylacetamide being particularly preferred. The reaction ratio of the compound represented by formula (4) to the compound represented by formula (5) can be appropriately set depending on the structure of the desired compound represented by formula (6). The reaction temperature is not particularly limited, but is preferably, for example, 0°C to the boiling point of the reaction solvent. The reaction time is not particularly limited, but can be, for example, 1 hour to 48 hours.

[0113] (Polymer (specific polymer) containing a structure derived from the compound represented by formula (1)) As the ultraviolet absorber, a polymer (specific polymer) containing a structure derived from the compound represented by formula (1) can also be used.

[0114] The specific polymer is a compound represented by the above formula (1), 1 , R 2 , Q 1 and Q 2 It is preferable that the compound contains a structure derived from a compound in which at least one of R is a group containing a polymerizable group having an ethylenically unsaturated bond (hereinafter also referred to as structure (1)). 11 , R 12 , Q 3 and Q 4 It is more preferable that the compound contains a structure derived from a compound having a structure in which at least one of the above is a group containing a polymerizable group having an ethylenically unsaturated bond (hereinafter also referred to as structure (3)).

[0115] The specific polymer may contain, in addition to the structure derived from the compound represented by formula (1), a structure derived from a compound having an ethylenically unsaturated bond-containing group other than the compound represented by formula (1) (hereinafter, also referred to as other polymerizable compound). 1 , R 2 , Q 1and Q 2 The copolymer may be a copolymer of a compound represented by formula (1) having a structure in which at least one of the groups is a group containing a polymerizable group having an ethylenically unsaturated bond, and another polymerizable compound. Examples of the other polymerizable compound include the polymerizable compounds described below as materials used in the composition of the present invention. Furthermore, as the other polymerizable compound, an ultraviolet absorber having a polymerizable group (also referred to as an other polymerizable ultraviolet absorber) other than the compound represented by formula (1) may also be used.

[0116] Examples of the polymerizable group contained in the other polymerizable ultraviolet absorber include a vinyl group, an allyl group, a (meth)acryloyl group, a (meth)acryloyloxy group, a (meth)acryloylamino group, a vinylphenyl group, etc. Examples of the other polymerizable ultraviolet absorber include an aminobutadiene compound, a dibenzoylmethane compound, a benzophenone compound, a benzotriazole compound, and a hydroxyphenyltriazine compound.

[0117] The content of the structure derived from the compound represented by formula (1) in the specific polymer is preferably 0.01 to 100% by mass. The upper limit is more preferably 50% by mass or less, and even more preferably 30% by mass or less. The lower limit is more preferably 0.02% by mass or more, and even more preferably 0.1% by mass or more.

[0118] The number weight average molecular weight of the specific polymer is preferably 5,000 to 150,000, more preferably 10,000 to 120,000, and even more preferably 20,000 to 100,000.

[0119] <<<Other UV Absorbents>>> The composition of the present invention may contain an UV absorbent other than the specific UV absorbent described above (hereinafter also referred to as an "other UV absorbent"). According to this aspect, it is possible to form a cured product that can block light with a wide range of wavelengths in the ultraviolet region.

[0120] The maximum absorption wavelength of the other ultraviolet absorber is preferably in the wavelength range of 300 to 380 nm, more preferably in the wavelength range of 300 to 370 nm, still more preferably in the wavelength range of 310 to 360 nm, and particularly preferably in the wavelength range of 310 to 350 nm.

[0121] The other ultraviolet absorber is also preferably a compound having a polymerizable group, such as a vinyl group, an allyl group, a (meth)acryloyl group, a (meth)acryloyloxy group, a (meth)acryloylamino group, or a vinylphenyl group.

[0122] As other ultraviolet absorbents, can be enumerated aminobutadiene-based ultraviolet absorbents, dibenzoylmethane-based ultraviolet absorbents, benzotriazole-based ultraviolet absorbents, benzophenone-based ultraviolet absorbents, salicylic acid-based ultraviolet absorbents, acrylate-based ultraviolet absorbents and triazine-based ultraviolet absorbents, and preferably benzotriazole-based ultraviolet absorbents, benzophenone-based ultraviolet absorbents and triazine-based ultraviolet absorbents, and more preferably benzotriazole-based ultraviolet absorbents and triazine-based ultraviolet absorbents.Specific examples of other ultraviolet absorbents can be enumerated compounds described in the examples below. Other ultraviolet absorbers are described in paragraphs 0065 to 0070 of JP 2009-263616 A, paragraph 0065 of WO 2017 / 122503 A, JP 2003-128730 A, JP 2003-129033 A, JP 2014-077076 A, JP 2015-164994 A, JP 2015-168822 A, JP 2018-135282 A, JP 2018-168089 A, JP 2018-168278 A, JP 2018-188589 A, JP 2019-001767 A, JP 2020-023697 A , JP 2020-041013 A, JP 5518613 A, JP 5868465 A, JP 6301526 A, JP 6354665 A, JP 2017-503905 A, WO 2015 / 064674, WO 2015 / 064675, WO 2017 / 102675, WO 2018 / 190281, WO 2018 / 216750, WO 2019 / 087983, EP 2379512 specification, compounds described in EP 2951163 specification, etc. can be used.

[0123] The content of the ultraviolet absorber in the total solid content of the composition is preferably 0.01 to 95% by mass. The lower limit can be 0.05% by mass or more, 0.1% by mass or more, 1% by mass or more, 5% by mass or more, 10% by mass or more, 20% by mass or more, 25% by mass or more, or 30% by mass or more. The upper limit can be 90% by mass or less, 80% by mass or less, 70% by mass or less, 60% by mass or less, 50% by mass or less, 40% by mass or less, 30% by mass or less, or 20% by mass or less. The content of the specific ultraviolet absorber in the ultraviolet absorber is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 20% by mass or more. The upper limit can be 100% by mass or less, 75% by mass or less, or 50% by mass or less.

[0124] The content of the specific ultraviolet absorber in the total solid content of the composition is preferably 0.01 to 50% by mass. The lower limit is preferably 0.05% by mass or more, and more preferably 0.1% by mass or more. The upper limit is preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less.

[0125] When the above-mentioned specific compound (compound represented by formula (1)) is used as the specific ultraviolet absorber, the content of the specific compound in the total solid content of the composition is preferably 0.01 to 50 mass%. The lower limit is preferably 0.05 mass% or more, and more preferably 0.1 mass% or more. The upper limit is preferably 40 mass% or less, more preferably 30 mass% or less, and even more preferably 20 mass% or less.

[0126] When the above-mentioned specific polymer (a polymer containing a structure derived from the compound represented by formula (1)) is used as the specific ultraviolet absorber, the content of the specific polymer in the total solid content of the composition is preferably 10 to 95% by mass. The lower limit is preferably 15% by mass or more, and more preferably 25% by mass or more. The upper limit is preferably 90% by mass or less, more preferably 85% by mass or less, and even more preferably 75% by mass or less.

[0127] The composition of the present invention may contain only one type of ultraviolet absorber, or may contain two or more types. When two or more types of ultraviolet absorbers are contained, the total amount thereof is preferably within the above range.

[0128] <<Anti-Fade Agent>> The composition of the present invention contains an anti-fading agent. The anti-fading agent used includes at least one selected from an amine compound, a phenol compound, a hydroquinone compound, a catechol compound, an ascorbic acid compound, a carotenoid compound, a metal complex compound, and a benzolactone compound. The amine compound is preferably a hydroxyamine compound, a tertiary amine compound, or an aminooxyl compound, more preferably a tertiary amine compound or an aminooxyl compound. The metal complex compound is preferably a Ni complex compound or a Co complex compound, more preferably a Ni complex compound. The anti-fading agent is preferably at least one selected from an amine compound and a benzolactone compound, more preferably an amine compound.

[0129] The anti-fading agent preferably contains at least one selected from the group consisting of a compound represented by formula (Ao1-1) and a compound represented by formula (Ao2-1), and more preferably contains a compound represented by formula (Ao1-1). In formula (Ao1-1), R a1 ~R a4 each independently represents a hydrogen atom, an alkyl group, or an alkenyl group; a1represents a hydrogen atom, an alkyl group, an alkenyl group, an alkoxy group, an alkenyloxy group, an alkoxycarbonyl group, an alkenyloxycarbonyl group, an aryloxycarbonyl group, an acyl group, an acyloxy group, an alkoxycarbonyloxy group, an alkenyloxycarbonyloxy group, an aryloxycarbonyloxy group, an alkylsulfonyl group, an alkenylsulfonyl group, an arylsulfonyl group, an alkylsulfinyl group, an alkenylsulfinyl group, an arylsulfinyl group, a sulfamoyl group, a carbamoyl group, a hydroxy group or an oxy radical group; X a2 represents an atomic group necessary to form a 5- to 7-membered ring; p1 represents a hydrogen atom, an alkyl group, an alkenyl group, an aryl group, a heterocyclic group, an acyl group, an alkoxycarbonyl group, an alkenyloxycarbonyl group, an aryloxycarbonyl group, an alkylsulfonyl group, an arylsulfonyl group, or —Si(R p101 ) (R p102 ) (R p103 ) and R p101 ~R p103 each independently represents an alkyl group, an alkenyl group, an aryl group, an alkoxy group, an alkenyloxy group, or an aryloxy group; R p2 ~R p6 each independently represents a hydrogen atom or a substituent, p1 ~R p6 two adjacent groups among R may be bonded to form a ring; p1 ~R p6 cannot all be hydrogen atoms.

[0130] The above groups in formula (Ao1-1) and formula (Ao1-2) may have a substituent. Examples of the substituent include the groups exemplified above for the substituent T.

[0131] -Regarding the compound represented by formula (Ao1-1)- R in formula (Ao1-1) a1 ~R a4are each independently preferably an alkyl group or an alkenyl group, more preferably an alkyl group. The alkyl group preferably has 1 to 5 carbon atoms, more preferably 1 to 3 carbon atoms. The alkyl group may be linear, branched, or cyclic, but is preferably linear. The alkyl group may have a substituent. Examples of the substituent include the groups listed above for the substituent T. The alkenyl group preferably has 2 to 5 carbon atoms, more preferably 2 or 3 carbon atoms. The alkenyl group is preferably linear or branched, more preferably linear. The alkenyl group may have a substituent. Examples of the substituent include the groups listed above for the substituent T.

[0132] R a1 ~R a4 is particularly preferably a methyl group.

[0133] X in formula (Ao1-1) a1is preferably a hydrogen atom, an oxy radical group, an alkyl group, an alkoxy group, an alkenyl group, an acyl group, or an aryl group, and more preferably an oxy radical group or an alkoxy group. The alkyl group preferably has 1 to 20 carbon atoms, and more preferably 1 to 12 carbon atoms. The alkyl group may be linear, branched, or cyclic, but is preferably linear. The alkyl group may have a substituent. Examples of the substituent include the groups listed above for substituent T. The alkenyl group preferably has 2 to 20 carbon atoms, and more preferably 2 to 12 carbon atoms. The alkenyl group is preferably linear or branched, and more preferably linear. The alkenyl group may have a substituent. Examples of the substituent include the groups listed above for substituent T. The alkoxy group preferably has 1 to 20 carbon atoms, and more preferably 1 to 12 carbon atoms. The alkoxy group is preferably linear or branched, and more preferably linear. The alkoxy may have a substituent. Examples of the substituent include the groups listed above for substituent T. The acyl group preferably has 2 to 20 carbon atoms, and more preferably 2 to 14 carbon atoms. The acyl group may have a substituent. Examples of the substituent include the groups exemplified above for the substituent T. The number of carbon atoms in the aryl group is preferably 6 to 20. The aryl group may have a substituent. Examples of the substituent include the groups exemplified above for the substituent T.

[0134] The compound represented by formula (Ao1-1) is preferably a compound represented by formula (Ao1-2). In formula (Ao1-2), X a11 represents a hydrogen atom, an alkyl group, an alkenyl group, an alkoxy group, an alkenyloxy group, an alkoxycarbonyl group, an alkenyloxycarbonyl group, an aryloxycarbonyl group, an acyl group, an acyloxy group, an alkoxycarbonyloxy group, an alkenyloxycarbonyloxy group, an aryloxycarbonyloxy group, an alkylsulfonyl group, an alkenylsulfonyl group, an arylsulfonyl group, an alkylsulfinyl group, an alkenylsulfinyl group, an arylsulfinyl group, a sulfamoyl group, a carbamoyl group, a hydroxy group, or an oxy radical group; R a11 represents a substituent;

[0135] X in formula (Ao1-2) a11 is X in formula (Ao1-1). a1 The same applies to the preferred range.

[0136] R in formula (Ao1-2) a11 Examples of the substituent represented by include the groups exemplified above as the substituent T. Examples of the alkyl group include an alkyl group, an alkenyl group, an alkynyl group, an aryl group, a heterocyclic group, a cyano group, a hydroxy group, a nitro group, a carboxy group, an alkoxy group, an aryloxy group, a silyloxy group, a heterocyclic oxy group, an acyloxy group, a carbamoyloxy group, an alkoxycarbonyloxy group, an aryloxycarbonyloxy group, an amino group, an acylamino group, an aminocarbonylamino group, an alkoxycarbonylamino group, an aryloxycarbonylamino group, a sulfamoylamino group, an alkylsulfonylamino group, an arylsulfonylamino group, a mercapto group, an alkylthio group, an arylthio group, a heterocyclic thio group, a sulfamoyl group, a sulfo group, an alkylsulfinyl group, an arylsulfinyl group, an alkylsulfonyl group, an arylsulfonyl group, an acyl group, an aryloxycarbonyl group, an alkoxycarbonyl group, a carbamoyl group, an arylazo group, a heterocyclic azo group, an imido group, a phosphino group, a phosphinyl group, a phosphinyloxy group, a phosphinylamino group, and a silyl group.

[0137] The compound represented by formula (Ao1-1) is preferably a compound represented by formula (Ao1-3). In formula (Ao1-3), X a21 represents a hydrogen atom, an alkyl group, an alkenyl group, an alkoxy group, an alkenyloxy group, an alkoxycarbonyl group, an alkenyloxycarbonyl group, an aryloxycarbonyl group, an acyl group, an acyloxy group, an alkoxycarbonyloxy group, an alkenyloxycarbonyloxy group, an aryloxycarbonyloxy group, an alkylsulfonyl group, an alkenylsulfonyl group, an arylsulfonyl group, an alkylsulfinyl group, an alkenylsulfinyl group, an arylsulfinyl group, a sulfamoyl group, a carbamoyl group, a hydroxy group or an oxy radical group; L a21represents a single bond or a divalent linking group; a22 represents an n-valent group, and n represents an integer of 1 or more.

[0138] X in formula (Ao1-3) a21 is X in formula (Ao1-1). a1 The same applies to the preferred range.

[0139] L in formula (Ao1-3) a21 The divalent linking group represented by the formula (I) includes -O-, -CO-, -COO-, -OCO-, -NHCO-, -NHCOO-, -CONH-, -OCONH-, -S-, and -SO 2 - and - OSO 2 - are some examples.

[0140] L in formula (Ao1-3) a22 represents an n-valent group. a22 When the n-valent group represented by is a monovalent group (when n is 1), L a22 Examples of the n-valent group represented by include an alkyl group, an alkenyl group, an alkynyl group, an aryl group, a heterocyclic group, a cyano group, a hydroxy group, a nitro group, a carboxy group, an alkoxy group, an aryloxy group, a silyloxy group, a heterocyclic oxy group, an acyloxy group, a carbamoyloxy group, an alkoxycarbonyloxy group, an aryloxycarbonyloxy group, an amino group, an acylamino group, an aminocarbonylamino group, an alkoxycarbonylamino group, an aryloxycarbonylamino group, a sulfamoylamino group, an alkyls Examples of the alkyl group include a sulfonylamino group, an arylsulfonylamino group, a mercapto group, an alkylthio group, an arylthio group, a heterocyclic thio group, a sulfamoyl group, a sulfo group, an alkylsulfinyl group, an arylsulfinyl group, an alkylsulfonyl group, an arylsulfonyl group, an acyl group, an aryloxycarbonyl group, an alkoxycarbonyl group, a carbamoyl group, an arylazo group, a heterocyclic azo group, an imido group, a phosphino group, a phosphinyl group, a phosphinyloxy group, a phosphinylamino group, and a silyl group.

[0141] L a22 When the n-valent group represented by is a divalent or higher valent group (when n is an integer of 2 or more), L a22Examples of the n-valent group represented by include hydrocarbon groups; and groups in which two or more hydrocarbon groups are bonded via -O-, -CO-, -COO-, -OCO-, -NH-, -S-, or a group combining two or more of these. Examples of the hydrocarbon group include aliphatic hydrocarbon groups and aromatic hydrocarbon groups, with aliphatic hydrocarbon groups being preferred. The aliphatic hydrocarbon group preferably has 1 to 30 carbon atoms, more preferably 1 to 20, and even more preferably 1 to 15. The aliphatic hydrocarbon group may be linear, branched, or cyclic, with linear or branched being preferred. The aliphatic hydrocarbon group may be either saturated or unsaturated, with saturated aliphatic hydrocarbon groups being preferred. The aromatic hydrocarbon group preferably has 6 to 30 carbon atoms, more preferably 6 to 20, and even more preferably 6 to 10. The hydrocarbon group may have a substituent. Examples of the substituent include a halogen atom, a hydroxy group, an alkyl group, and an aryl group.

[0142] When the n-valent group is a divalent or higher valent group, L a22 The n-valent linking group represented by is preferably a group containing a saturated aliphatic hydrocarbon group having 1 to 20 carbon atoms (preferably 2 to 15 carbon atoms, more preferably 2 to 10 carbon atoms).

[0143] In formula (Ao1-3), n represents an integer of 1 or more, preferably an integer of 2 or more, more preferably an integer of 2 to 6, and even more preferably an integer of 2 to 4.

[0144] -Regarding the compound represented by formula (Ao2-1)- R in formula (Ao2-1) p1 represents a hydrogen atom, an alkyl group, an alkenyl group, an aryl group, a heterocyclic group, an acyl group, an alkoxycarbonyl group, an alkenyloxycarbonyl group, an aryloxycarbonyl group, an alkylsulfonyl group, an arylsulfonyl group, or —Si(R p101 ) (R p102 ) (R p103 ) and R p101 ~R p103 R each independently represents an alkyl group, an alkenyl group, an aryl group, an alkoxy group, an alkenyloxy group, or an aryloxy group. p1is preferably a hydrogen atom, an alkyl group or an acyl group, more preferably an alkyl group or an acyl group.

[0145] R p2 ~R p6 Examples of the substituent represented by the formula (I) include a halogen atom, an alkyl group, an alkenyl group, an alkynyl group, an aryl group, a heterocyclic group, a cyano group, a hydroxy group, a nitro group, a carboxy group, an alkoxy group, an aryloxy group, a silyloxy group, a heterocyclic oxy group, an acyloxy group, a carbamoyloxy group, an alkoxycarbonyloxy group, an aryloxycarbonyloxy group, an amino group, an acylamino group, an aminocarbonylamino group, an alkoxycarbonylamino group, an aryloxycarbonylamino group, a sulfamoylamino group, an alkylsulfonylamino group, an arylsulfonylamino group, a mercapto group, an alkylthio group, an arylthio group, a heterocyclic thio group, a sulfamoyl group, a sulfo Examples of the alkyl group include alkylsulfinyl groups, arylsulfinyl groups, alkylsulfonyl groups, arylsulfonyl groups, acyl groups, aryloxycarbonyl groups, alkoxycarbonyl groups, carbamoyl groups, arylazo groups, heterocyclic azo groups, imido groups, phosphino groups, phosphinyl groups, phosphinyloxy groups, phosphinylamino groups, and silyl groups. The alkyl group is preferably an alkyl group, an alkenyl group, an aryl group, an alkoxy group, an alkoxycarbonyl group, an aryloxy group, an aryloxycarbonyl group, an alkylsulfonyl group, or an arylsulfonyl group, more preferably an alkyl group or an alkenyl group, and even more preferably an alkyl group. The alkyl group preferably has 1 to 10 carbon atoms, more preferably 1 to 5 carbon atoms. The alkyl group may be linear, branched, or cyclic, but is preferably linear or branched, and more preferably branched. The alkyl group may have a substituent. Examples of the substituent include the groups listed above for the substituent T. The alkenyl group preferably has 2 to 10 carbon atoms, more preferably 2 to 5 carbon atoms. The alkenyl group is preferably linear or branched, and more preferably branched. The alkenyl group may have a substituent. Examples of the substituent include the groups exemplified above for the substituent T.

[0146] Rp2 ~R p6 At least one of the groups is preferably a substituent, and two or more of the groups are more preferably substituents.

[0147] In formula (Ao2-1), R p1 ~R p6 Among these, two adjacent groups may be bonded to form a ring. The ring formed is preferably a 5-membered or 6-membered ring. The ring formed may further have a substituent. Examples of the substituent include the groups listed above for the substituent T and ethylenically unsaturated bond-containing groups. Examples of the ethylenically unsaturated bond-containing group include a vinyl group.

[0148] As a preferred embodiment of formula (Ao2-1), R p1 and R p2 and bonded to form a ring. The ring formed is preferably a 5-membered or 6-membered ring. The ring formed preferably further has a substituent. Examples of the substituent include an aryl group, a heteroaryl group, and an ethylenically unsaturated bond-containing group, with an aryl group and an ethylenically unsaturated bond-containing group being preferred, and an aryl group being more preferred. The aryl group and the heteroaryl group may further have a substituent. Examples of the further substituent include an alkyl group, an alkenyl group, an aryl group, an alkoxy group, an alkenyloxy group, an aryloxy group, an acyl group, and a hydroxy group.

[0149] In formula (Ao2-1), R p1 ~R p6 Not all of R are hydrogen atoms. p1 ~R p6 The total number of carbon atoms is preferably 10 or more, and more preferably 16 or more.

[0150] The compound represented by formula (Ao2-1) is preferably a compound represented by formula (Ao2-2). In formula (Ao2-2), R p11 ~R p14 each independently represents a hydrogen atom, an alkyl group, or an alkenyl group; Y p11represents an aryl group, a heteroaryl group, or an ethylenically unsaturated bond-containing group.

[0151] R p11 ~R p14 The number of carbon atoms in the alkyl group represented by is preferably 1 to 10, more preferably 1 to 5. The alkyl group may be linear, branched, or cyclic, but is preferably linear or branched, more preferably branched. The alkyl group may have a substituent. Examples of the substituent include the groups listed above for the substituent T. R p11 ~R p14 The number of carbon atoms in the alkenyl group represented by is preferably 2 to 10, more preferably 2 to 5. The alkenyl group is preferably linear or branched, more preferably branched. The alkenyl group may have a substituent. Examples of the substituent include the groups listed above for the substituent T.

[0152] R p11 ~R p14 It is preferable that at least one of R is an alkyl group or an alkenyl group, and it is more preferable that two or more of R are alkyl groups or alkenyl groups. p11 ~R p14 At least one of the groups is preferably an alkyl group, and more preferably two or more of the groups are alkyl groups.

[0153] Y p11 represents an aryl group, a heteroaryl group, or an ethylenically unsaturated bond-containing group, and is preferably an aryl group. The aryl group and heteroaryl group may further have a substituent. Examples of the further substituent include an alkyl group, an alkenyl group, an aryl group, an alkoxy group, an alkenyloxy group, an aryloxy group, an acyl group, and a hydroxy group. Examples of the ethylenically unsaturated bond-containing group include a vinyl group.

[0154] The compound represented by formula (Ao2-1) is preferably a compound represented by formula (Ao2-3). In formula (Ao2-3), R p21 ~R p24 each independently represents a hydrogen atom, an alkyl group, or an alkenyl group; Rp25 represents an alkyl group, an alkenyl group, or a hydroxy group; L p21 represents an s-valent group, r represents an integer of 0 to 4, s represents an integer of 1 or more, and when r is an integer of 2 or more, there are r R p25 may be the same or different.

[0155] R in formula (Ao2-3) p21 ~R p24 is R in formula (Ao2-2) p11 ~R p14 The same definition and preferred range are also true. p21 ~R p24 It is preferable that at least one of R is an alkyl group or an alkenyl group, and it is more preferable that two or more of R are alkyl groups or alkenyl groups. p21 ~R p24 At least one of the groups is preferably an alkyl group, and more preferably two or more of the groups are alkyl groups.

[0156] R in formula (Ao2-3) p25 is preferably an alkyl group or an alkenyl group, more preferably an alkyl group. The number of carbon atoms in the alkyl group is preferably 1 to 10, more preferably 1 to 5. The alkyl group may be linear, branched, or cyclic, but is preferably linear or branched, more preferably branched. The alkyl group may have a substituent. Examples of the substituent include the groups listed above for the substituent T. The number of carbon atoms in the alkenyl group is preferably 2 to 10, more preferably 2 to 5. The alkenyl group is preferably linear or branched, more preferably branched. The alkenyl group may have a substituent. Examples of the substituent include the groups listed above for the substituent T. p21 represents an s-valent group. p21 When the s-valent group represented by is a monovalent group, L p21 Examples of the s-valent group represented by L include an alkyl group, an alkenyl group, an alkoxy group, and an alkynyl group, and an alkyl group or an alkoxy group is preferred. p21 When the s-valent group represented by is a divalent or higher valent group, L p21The s-valent group represented by the formula (I) includes a hydrocarbon group, -O-, -CO-, -COO-, -OCO-, -NHCO-, -NHCOO-, -CONH-, -OCONH-, -S-, and -SO 2 --OSO 2 - and groups formed by combining two or more of these groups. Examples of the hydrocarbon group include aliphatic hydrocarbon groups and aromatic hydrocarbon groups. The aliphatic hydrocarbon group preferably has 1 to 30 carbon atoms, more preferably 1 to 20 carbon atoms, and even more preferably 1 to 15 carbon atoms. The aliphatic hydrocarbon group may be linear, branched, or cyclic, but is preferably linear or branched. The aliphatic hydrocarbon group may be either a saturated aliphatic hydrocarbon group or an unsaturated aliphatic hydrocarbon group, but is preferably a saturated aliphatic hydrocarbon group. The aromatic hydrocarbon group preferably has 6 to 30 carbon atoms, more preferably 6 to 20 carbon atoms, and even more preferably 6 to 10 carbon atoms. The hydrocarbon group may have a substituent. Examples of the substituent include a halogen atom, a hydroxy group, an alkyl group, and an aryl group.

[0157] r represents an integer of 0 to 4, and preferably an integer of 0 to 2. s represents an integer of 1 or more, and preferably an integer of 1 to 4, and more preferably 1 or 2.

[0158] Specific examples of the anti-fading agent include the compounds described in the examples below, the compounds described in paragraphs 0157 to 0171 of JP-A-2009-067984, and compounds having the structures shown below.

[0159] The content of the anti-fading agent in the total solid content of the composition is preferably 0.01 to 50% by mass. The lower limit is preferably 0.05% by mass or more, and more preferably 0.1% by mass or more. The upper limit is preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less.

[0160] The content of the anti-fading agent is preferably 0.1 to 500 parts by mass relative to 100 parts by mass of the ultraviolet absorber. The upper limit is preferably 300 parts by mass or less, more preferably 200 parts by mass or less. The lower limit is preferably 1 part by mass or more, more preferably 10 parts by mass or more.

[0161] The content of the anti-fading agent is preferably 0.1 to 500 parts by mass relative to 100 parts by mass of the above-mentioned specific ultraviolet absorber. The upper limit is preferably 300 parts by mass or less, more preferably 200 parts by mass or less. The lower limit is preferably 1 part by mass or more, more preferably 10 parts by mass or more.

[0162] The composition of the present invention may contain only one type of anti-fading agent, or may contain two or more types. When two or more anti-fading agents are contained, the total amount thereof is preferably within the above range.

[0163] <<Curable Compound>> The composition of the present invention contains a curable compound. Examples of the curable compound include polymerizable compounds and resins. The resin may be a non-polymerizable resin (a resin without a polymerizable group) or a polymerizable resin (a resin with a polymerizable group). Examples of the polymerizable group include an ethylenically unsaturated bond-containing group and a cyclic ether group. Examples of the ethylenically unsaturated bond-containing group include a vinyl group, a vinylphenyl group, a (meth)allyl group, a (meth)acryloyl group, a (meth)acryloyloxy group, and a (meth)acryloylamide group. Preferred are a (meth)allyl group, a (meth)acryloyl group, and a (meth)acryloyloxy group, and more preferred are a (meth)acryloyloxy group. Examples of the cyclic ether group include an epoxy group and an oxetanyl group, and preferred is an epoxy group.

[0164] The curable compound contained in the composition of the present invention preferably contains at least one selected from a resin and a polymerizable compound. The curable compound may be a combination of a resin and a polymerizable compound.

[0165] (Polymerizable Compound) As the polymerizable compound, any compound that can be polymerized and cured by the application of energy can be used without limitation. The polymerizable compound may be a radical polymerizable compound or a cation polymerizable compound.

[0166] The polymerizable compound may be any of a monomer, a prepolymer (i.e., a dimer, a trimer, or an oligomer), a mixture thereof, and a (co)polymer of a compound selected from a monomer and a prepolymer, but is preferably a monomer.

[0167] The molecular weight of the polymerizable compound is preferably 100 to 3000. The upper limit is preferably 2000 or less, more preferably 1500 or less. The lower limit is preferably 150 or more, more preferably 250 or more.

[0168] -Radical Polymerizable Compound- Examples of the radical polymerizable compound include compounds having an ethylenically unsaturated bond-containing group. Examples of the radical polymerizable compound include unsaturated carboxylic acids (e.g., acrylic acid, methacrylic acid, itaconic acid, crotonic acid, isocrotonic acid, maleic acid, etc.), esters of unsaturated carboxylic acids, amides of unsaturated carboxylic acids, and (co)polymers of unsaturated carboxylic acids or their esters or amides. Among these, esters of unsaturated carboxylic acids and aliphatic polyhydric alcohols, amides of unsaturated carboxylic acids and aliphatic polyamines, and homopolymers or copolymers thereof are preferred.

[0169] Examples of radically polymerizable compounds that can be used include an addition reaction product of an unsaturated carboxylic acid ester or unsaturated carboxylic acid amide having a nucleophilic substituent (e.g., a hydroxy group, an amino group, a mercapto group, etc.) with a monofunctional or polyfunctional isocyanate compound or an epoxy compound; a dehydration condensation reaction product of an unsaturated carboxylic acid ester or unsaturated carboxylic acid amide having a nucleophilic substituent with a monofunctional or polyfunctional carboxylic acid; an addition reaction product of an unsaturated carboxylic acid ester or unsaturated carboxylic acid amide having an electrophilic substituent (e.g., an isocyanate group, an epoxy group, etc.) with a monofunctional or polyfunctional alcohol, amine, or thiol; and a substitution reaction product of an unsaturated carboxylic acid ester or unsaturated carboxylic acid amide having a leaving substituent (e.g., a halogen atom, a tosyloxy group, etc.) with a monofunctional or polyfunctional alcohol, amine, or thiol. Furthermore, compounds obtained by replacing the above unsaturated carboxylic acid with an unsaturated phosphonic acid, styrene, vinyl ether, etc. can also be used.

[0170] The radical polymerizable compound may be a combination of a plurality of compounds having different functionalities or a plurality of compounds having different types of polymerizable groups (e.g., acrylic acid esters, methacrylic acid esters, styrene compounds, vinyl ether compounds, etc.).

[0171] The radical polymerizable compound is preferably a (meth)acrylate compound, more preferably a di- or higher functional (meth)acrylate compound, even more preferably a di- to 15-functional (meth)acrylate compound, still more preferably a di- to 10-functional (meth)acrylate compound, and particularly preferably a di- to hexa-functional (meth)acrylate compound.

[0172] Specific examples of the radical polymerizable compound include pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tri((meth)acryloyloxyethyl)isocyanurate, pentaerythritol tetra(meth)acrylate ethylene oxide EO (ethylene oxide) modified product, dipentaerythritol hexa(meth)acrylate EO (ethylene oxide) modified product, and benzyl (meth)acrylate.

[0173] Commercially available radically polymerizable compounds include polyfunctional (meth)acrylate compounds such as the KAYARAD series (e.g., D-330, D-320, D-310, PET-30, TPA-330, DPHA, etc.) manufactured by Nippon Kayaku Co., Ltd., the NK Ester series (e.g., A-DPH-12E, A-TMMT, A-TMM-3, etc.) manufactured by Shin-Nakamura Chemical Co., Ltd., the Light Acrylate series (e.g., DCP-A, etc.) manufactured by Kyoeisha Chemical Co., Ltd., the Aronix series (e.g., M-305, M-306, M-309, M-450, M-402, TO-1382, etc.) manufactured by Toagosei Co., Ltd., and the Viscoat series (e.g., V#802, etc.) manufactured by Osaka Organic Chemical Industry Ltd.

[0174] The radical polymerizable compound may be a (meth)acrylate compound described in JP-A-48-064183, JP-B-49-043191, or JP-B-52-030490, or a compound introduced as a photocurable monomer or oligomer in Journal of the Japan Adhesion Association, Vol. 20, No. 7, pp. 300-308 (1984).

[0175] -Cationically polymerizable compound- Examples of the cationically polymerizable compound include compounds having a cationically polymerizable group. Examples of the cationically polymerizable group include cyclic ether groups such as epoxy groups and oxetanyl groups, and vinyl ether groups, with a cyclic ether group being preferred. Furthermore, the cationically polymerizable compound is preferably a polyfunctional cationically polymerizable compound having two or more cationically polymerizable groups.

[0176] Examples of the cationically polymerizable compound include polyfunctional alicyclic epoxy compounds, polyfunctional heterocyclic epoxy compounds, polyfunctional oxetane compounds, alkylene glycol diglycidyl ethers, and alkylene glycol monovinyl monoglycidyl ethers.

[0177] Specific examples of the cationically polymerizable compound include 3',4'-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate, bisphenol A diglycidyl ether, hydrogenated bisphenol A diglycidyl ether, 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexanecarboxylate, 1,2-epoxy-4-(2-oxiranyl)cyclohexane adduct of 2,2-bis(hydroxymethyl)-1-butanol, xylylene bisoxetane, 3-ethyl-3-hydroxymethyloxetane, 3-ethyl-3-{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane, cyclohexanedimethanol divinyl ether, 2-ethylhexyl vinyl ether, cyclohexanedimethanol monovinyl ether, 4-hydroxybutyl vinyl ether, and the compounds described in paragraphs 0029 to 0058 of JP-A 2012-046577.

[0178] The cationically polymerizable compound may also be a (meth)acrylate compound having a cationically polymerizable group. Specific examples of (meth)acrylate compounds having a cationically polymerizable group include 3,4-epoxycyclohexylmethyl methacrylate. Commercially available products include Cyclomer M100 manufactured by Daicel Corporation.

[0179] Examples of the cationically polymerizable compound that can be used include the Aron Oxetane series (OXT-101, OXT-121, OXT-221, etc.) manufactured by Toagosei Co., Ltd., the Celloxide series (2021P) manufactured by Daicel Corporation, and alkyl divinyl ether CHDVE, alkyl monovinyl ether EHVE, hydroxyalkyl vinyl ether CHMVE, and hydroxyalkyl vinyl ether HBVE manufactured by Nippon Carbide Industries Co., Ltd. In addition, the compounds exemplified below as specific examples of epoxy resins can also be used.

[0180] (Resin) Examples of resins include (meth)acrylic resins, ene-thiol resins, polyester resins, polycarbonate resins, vinyl polymers [e.g., polydiene resins, polyalkene resins, polystyrene resins, polyvinyl ether resins, polyvinyl alcohol resins, polyvinyl ketone resins, polyfluorovinyl resins, and polyvinyl bromide resins], polythioether resins, polyphenylene resins, polyurethane resins, polysulfonate resins, nitrosopolymer resins, polysiloxane resins, polysulfide resins, polythioester resins, polysulfone resins, polysulfonamide resins, polyamide resins, polyimine resins, polyurea resins, polyphosphazene resins, polysilane resins, polysilazane resins, polyfuran resins, and polybenzoxazo Examples of the resin include olefin resins, polyoxadiazole resins, polybenzothiazinophenothiazine resins, polybenzothiazole resins, polypyrazinoquinoxaline resins, polyquinoxaline resins, polybenzimidazole resins, polyoxoisoindoline resins, polydioxoisoindoline resins, polytriazine resins, polypyridazine resins, polypiperazine resins, polypyridine resins, polypiperidine resins, polytriazole resins, polypyrazole resins, polypyrrolidine resins, polycarborane resins, polyoxabicyclononane resins, polydibenzofuran resins, polyphthalide resins, polyacetal resins, polyimide resins, polyamideimide resins, olefin resins, cyclic olefin resins, epoxy resins, and cellulose acylate resins.

[0181] Examples of (meth)acrylic resins include polymers containing structural units derived from (meth)acrylic acid and / or its esters, specifically polymers obtained by polymerizing at least one compound selected from the group consisting of (meth)acrylic acid, (meth)acrylic acid esters, (meth)acrylamide, and (meth)acrylonitrile.

[0182] Examples of polyester resins include polymers obtained by reacting polyols (e.g., ethylene glycol, propylene glycol, glycerin, and trimethylolpropane) with polybasic acids (e.g., aromatic dicarboxylic acids (e.g., terephthalic acid, isophthalic acid, and naphthalenedicarboxylic acid, and dicarboxylic acids in which hydrogen atoms on these aromatic rings are substituted with methyl groups, ethyl groups, phenyl groups, etc.), aliphatic dicarboxylic acids having 2 to 20 carbon atoms (e.g., adipic acid, sebacic acid, and dodecanedicarboxylic acid), or alicyclic dicarboxylic acids (e.g., cyclohexanedicarboxylic acid)), as well as polymers obtained by ring-opening polymerization of cyclic ester compounds such as caprolactone monomers (e.g., polycaprolactone). Specific examples of polyester resins include polyethylene terephthalate and polyethylene naphthalate.

[0183] Examples of epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, aliphatic epoxy resins, etc. As the epoxy resin, commercially available products on the market may be used, and examples of commercially available products include the following:

[0184] Examples of commercially available bisphenol A epoxy resins include jER825, jER827, jER828, jER834, jER1001, jER1002, jER1003, jER1055, jER1007, jER1009, and jER1010 (all manufactured by Mitsubishi Chemical Corporation), and EPICLON860, EPICLON1050, EPICLON1051, and EPICLON1055 (all manufactured by DIC Corporation). Commercially available examples of bisphenol F epoxy resins include jER806, jER807, jER4004, jER4005, jER4007, and jER4010 (all manufactured by Mitsubishi Chemical Corporation), EPICLON830 and EPICLON835 (both manufactured by DIC Corporation), and LCE-21 and RE-602S (both manufactured by Nippon Kayaku Co., Ltd.). Commercially available examples of phenol novolac epoxy resins include jER152, jER154, jER157S70, and jER157S65 (all manufactured by Mitsubishi Chemical Corporation), and EPICLON N-740, EPICLON N-770, and EPICLON N-775 (all manufactured by DIC Corporation). Commercially available examples of cresol novolac epoxy resins include EPICLON N-660, EPICLON N-665, EPICLON N-670, EPICLON N-673, EPICLON N-680, EPICLON N-690, and EPICLON N-695 (all manufactured by DIC Corporation), and EOCN-1020 (manufactured by Nippon Kayaku Co., Ltd.).Commercially available examples of aliphatic epoxy resins include the ADEKA RESIN EP series (e.g., EP-4080S, EP-4085S, and EP-4088S; manufactured by ADEKA Corporation), CELLOXIDE 2021P, CELLOXIDE 2081, CELLOXIDE 2083, CELLOXIDE 2085, EHPE3150, EPOLEAD PB 3600, and EPOLEAD PB 4700 (manufactured by Daicel Corporation), DENACOL EX-212L, EX-214L, EX-216L, EX-321L, and EX-850L (manufactured by Nagase ChemteX Corporation), ADEKA RESIN Examples of such an adhesive include the EP series (e.g., EP-4000S, EP-4003S, EP-4010S, and EP-4011S manufactured by ADEKA Corporation), NC-2000, NC-3000, NC-7300, XD-1000, EPPN-501, and EPPN-502 (all manufactured by ADEKA Corporation), and jER1031S (manufactured by Mitsubishi Chemical Corporation). Other commercially available examples of epoxy resins include Marproof G-0150M, G-0105SA, G-0130SP, G-0250SP, G-1005S, G-1005SA, G-1010S, G-2050M, G-01100, and G-01758 (all manufactured by NOF Corporation, epoxy group-containing polymers).

[0185] As the cellulose acylate resin, cellulose acylate described in paragraphs 0016 to 0021 of JP-A No. 2012-215689 is preferably used. As the polyester resin, commercially available products such as the Vylon series (e.g., Vylon 500) manufactured by Toyobo Co., Ltd. can also be used. As a commercially available (meth)acrylic resin, the SK Dyne series (e.g., SK Dyne-SF2147) manufactured by Soken Chemical & Engineering Co., Ltd. can also be used.

[0186] The polystyrene resin is preferably a resin containing 50% by mass or more of repeating units derived from a styrene-based monomer, more preferably a resin containing 70% by mass or more of repeating units derived from a styrene-based monomer, and even more preferably a resin containing 85% by mass or more of repeating units derived from a styrene-based monomer.

[0187] Specific examples of styrene-based monomers include styrene and its derivatives. Here, the styrene derivative is a compound in which another group is bonded to styrene, and examples thereof include alkylstyrenes such as o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, o-ethylstyrene, and p-ethylstyrene, and substituted styrenes in which a hydroxyl group, an alkoxy group, a carboxyl group, a halogen, or the like is introduced into the benzene nucleus of styrene, such as hydroxystyrene, tert-butoxystyrene, vinylbenzoic acid, o-chlorostyrene, and p-chlorostyrene.

[0188] The polystyrene resin may also contain repeating units derived from monomers other than styrene-based monomers. Examples of such other monomers include alkyl (meth)acrylates such as methyl (meth)acrylate, cyclohexyl (meth)acrylate, methylphenyl (meth)acrylate, and isopropyl (meth)acrylate; unsaturated carboxylic acid monomers such as methacrylic acid, acrylic acid, itaconic acid, maleic acid, fumaric acid, and cinnamic acid; unsaturated dicarboxylic acid anhydride monomers such as maleic anhydride, itaconic acid, ethyl maleic acid, methyl itaconic acid, and chloromaleic acid; unsaturated nitrile monomers such as acrylonitrile and methacrylonitrile; and conjugated dienes such as 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, and 1,3-hexadiene.

[0189] Commercially available polystyrene resins include AS-70 (acrylonitrile-styrene copolymer resin) manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., SMA2000P (styrene-maleic acid copolymer) manufactured by Kawahara Oil Chemical Co., Ltd., Clearen 530L and Clearen 730L manufactured by Denka Co., Ltd., Tufprene 126S and Asaprene T411 manufactured by Asahi Kasei Corporation, Kraton D1102A and Kraton D1116A manufactured by Kraton Polymer Japan, Styrolux S and Styrolux T manufactured by Styrolution, Asaflex 840 and Asaflex 860 manufactured by Asahi Kasei Corporation, 679, HF77, SGP-10, 475D, H0103, and HT478 manufactured by PS Japan, and DIC Styrene XC-515, DIC Styrene XC-535, and DIC Styrene manufactured by DIC Corporation. GH-8300-5, etc. Commercially available hydrogenated polystyrene resins include the Tuftec H series manufactured by Asahi Kasei Corporation, the Kraton G series manufactured by Shell Japan, Dynaron (hydrogenated styrene-butadiene random copolymer) manufactured by JSR Corporation, and Septon manufactured by Kuraray Co., Ltd. Commercially available modified polystyrene resins include the Tuftec M series manufactured by Asahi Kasei Corporation, Epofriend manufactured by Daicel Corporation, polar group-modified Dynaron manufactured by JSR Corporation, and Reseda manufactured by Toagosei Co., Ltd.

[0190] Examples of cyclic olefin resins include (R1) polymers containing structural units derived from norbornene compounds, (R2) polymers containing structural units derived from monocyclic cyclic olefin compounds other than norbornene compounds, (R3) polymers containing structural units derived from cyclic conjugated diene compounds, (R4) polymers containing structural units derived from vinyl alicyclic hydrocarbon compounds, and hydrogenated polymers containing structural units derived from each of the compounds (R1) to (R4). In this specification, polymers containing structural units derived from norbornene compounds and polymers containing structural units derived from monocyclic cyclic olefin compounds include ring-opened polymers of each compound.

[0191] The cyclic olefin resin is not particularly limited, but is preferably a polymer having a structural unit derived from a norbornene compound represented by formula (A-II) or formula (A-III). The polymer having the structural unit represented by formula (A-II) is an addition polymer of a norbornene compound, and the polymer having the structural unit represented by formula (A-III) is a ring-opening polymer of a norbornene compound.

[0192]

[0193] In formula (A-II) and formula (A-III), m is an integer of 0 to 4, preferably 0 or 1. R in formula (A-II) and formula (A-III) 3 ~R 6 R each independently represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms. 3 ~R 6 Examples of the hydrocarbon group represented by X include an alkyl group, an alkenyl group, an alkynyl group, and an aryl group, and an alkyl group or an aryl group is preferred. 2 and X 3 , Y 2 and Y 3 each independently represents a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, a halogen atom, a hydrocarbon group having 1 to 10 carbon atoms substituted with a halogen atom, -(CH 2 ) n COOR 11 , -(CH 2 ) n OCOR 12 , -(CH 2 ) n NCO, -(CH 2 ) n NO 2 , -(CH 2 ) n CN, -(CH 2 ) n CONR 13 R 14 , -(CH 2 ) n NR 13 R 14 , -(CH 2 ) n OZ 1 , -(CH 2 ) n W1 , or X 2 and Y 2 or X 3 and Y 3 are bonded to each other to form (-CO) 2 O or (-CO) 2 NR 15 where X 2 , X 3 , Y 2 and Y 3 R in each of the above groups 11 ~R 15 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms; Z 1 represents a hydrocarbon group or a halogen-substituted hydrocarbon group; W 1 is Si(R 16 ) p D (3-p) (R 16 represents a hydrocarbon group having 1 to 10 carbon atoms, D represents a halogen atom, -OCOR 17 Or -OR 17 (R 17 represents a hydrocarbon group having 1 to 10 carbon atoms. p represents an integer of 0 to 3. n represents an integer of 0 to 10, preferably 0 to 8, and more preferably 0 to 6.

[0194] R in formula (A-II) and formula (A-III) 3 ~R 6 are each independently a hydrogen atom or —CH 3 is preferable, and from the viewpoint of moisture permeability, it is more preferable that X is a hydrogen atom. 2 and X 3 are hydrogen atoms, -CH 3 , -C 2 H 5 is preferable, and from the viewpoint of moisture permeability, a hydrogen atom is more preferable. 2 and Y 3 are each independently a hydrogen atom, a halogen atom (particularly a chlorine atom), or -(CH 2 ) n COOR 11 (Especially -COOCH 3 ) is preferable, and from the viewpoint of moisture permeability, a hydrogen atom is more preferable. The other groups are appropriately selected.

[0195] The polymer having the structural unit represented by formula (A-II) or formula (A-III) may further contain one or more structural units represented by formula (AI).

[0196]

[0197] In formula (AI), R 1 and R 2 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms; X 1 and Y 1 each independently represents a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, a halogen atom, a hydrocarbon group having 1 to 10 carbon atoms substituted with a halogen atom, -(CH 2 ) n COOR 11 , -(CH 2 ) n OCOR 12 , -(CH 2 ) n NCO, -(CH 2 ) n NO 2 , -(CH 2 ) n CN, -(CH 2 ) n CONR 13 R 14 , -(CH 2 ) n NR 13 R 14 , -(CH 2 ) n OZ 1 , -(CH 2 ) n W 1 , or X 2 and Y 2 or X 3 and Y 3 are bonded to each other to form (-CO) 2 O or (-CO) 2 NR 15 represents. 1 and Y 1 R in each of the above groups 11 ~R 15 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms; Z 1represents a hydrocarbon group or a halogen-substituted hydrocarbon group; W 1 is Si(R 16 ) p D (3-p) (R 16 represents a hydrocarbon group having 1 to 10 carbon atoms, D represents a halogen atom, -OCOR 17 Or -OR 17 (R 17 represents a hydrocarbon group having 1 to 10 carbon atoms. p represents an integer of 0 to 3. n represents an integer of 0 to 10.

[0198] The content of the structural unit represented by formula (A-II) or formula (A-III) in the cyclic polyolefin resin is preferably 90 mass% or less, more preferably 30 to 85 mass%, even more preferably 50 to 79 mass%, and still more preferably 60 to 75 mass%.

[0199] Cyclic olefin resins are described in JP-A No. 10-007732, JP-A No. 2002-504184, WO 2004 / 070463, etc., and the contents of these publications can be referred to as appropriate.

[0200] The cyclic olefin resin can be obtained by addition polymerization of norbornene compounds (for example, polycyclic unsaturated compounds of norbornene).

[0201] Commercially available cyclic olefin resins include the Arton series (for example, Arton G, F, and RX4500) manufactured by JSR Corporation, and Zeonor ZF14, ZF16, and Zeonex 250 and 280 manufactured by Zeon Corporation.

[0202] Examples of cyclic olefin resins include copolymers obtained by addition copolymerization of norbornene compounds with olefins such as ethylene, propylene, and butene, conjugated dienes such as butadiene and isoprene, non-conjugated dienes such as ethylidene norbornene, and ethylenically unsaturated compounds such as acrylonitrile, acrylic acid, methacrylic acid, maleic anhydride, acrylic acid esters, methacrylic acid esters, maleimide, vinyl acetate, and vinyl chloride. Among these, copolymers with ethylene are preferred. Examples of such addition (co)polymers of norbornene compounds include those sold by Mitsui Chemicals under the trade name APEL, which have different glass transition temperatures (Tg), such as APL8008T (Tg 70°C), APL6011T (Tg 105°C), APL6013T (Tg 125°C), and APL6015T (Tg 145°C). Polyplastics Co., Ltd. sells pellets such as TOPAS 8007, 6013, and 6015. Ferrania also sells Appear 3000.

[0203] Hydrogenated cyclic olefin resins can be synthesized by subjecting norbornene compounds, etc., to addition polymerization or metathesis ring-opening polymerization, followed by hydrogenation. Synthetic methods are described in, for example, JP-A Nos. 01-240517, 07-196736, 60-026024, 62-019801, 2003-159767, and 2004-309979.

[0204] The weight molecular weight of the cyclic olefin resin is preferably 5,000 to 500,000, more preferably 8,000 to 200,000, and even more preferably 10,000 to 100,000.

[0205] Examples of polycarbonate resins include reaction products of polyhydric phenol compounds with phosgene or carbonate compounds.

[0206] Examples of polyhydric phenol compounds include hydroquinone, resorcinol, 4,4'-dihydroxydiphenyl, bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, bisphenol A, bisphenol C, bisphenol E, bisphenol F, bisphenol M, bisphenol P, bisphenol S, bisphenol Z, 2,2-bis(3-methyl-4-hydroxyphenyl)propane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 2,2-bis(3-phenyl-4-hydroxyphenyl)propane, 2,2-bis( 3-isopropyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, 2,2-bis(3,5-dibromo-4-hydroxyphenyl)propane, 4,4'-dihydroxydiphenyl sulfone, 4,4'-dihydroxydiphenyl sulfoxide, 4,4'-dihydroxydiphenyl sulfide, 3,3'-dimethyl-4,4'-dihydroxydiphenyl sulfide, 4,4'-dihydroxydiphenyl oxide, and the like are listed, and hydroquinone, resorcinol, 4,4'-dihydroxydiphenyl, and bisphenol A are preferred.

[0207] Examples of the carbonate ester compound include phosgene, diphenyl carbonate, bis(chlorophenyl) carbonate, dinaphthyl carbonate, bis(diphenyl) carbonate, dimethyl carbonate, diethyl carbonate, and dibutyl carbonate, with bis(diphenyl) carbonate, dimethyl carbonate, and diethyl carbonate being preferred.

[0208] Commercially available polycarbonate resins include Panlite L-1250WP and Panlite SP-1516 manufactured by Teijin Limited, Iupizeta EP-5000 and Iupizeta EP-4000 manufactured by Mitsubishi Gas Chemical Company, Inc., and Caliber 301-30 manufactured by Sumika Polycarbonate Co., Ltd.

[0209] Examples of thiourethane resins include a reaction product of an isocyanate compound and a polythiol compound, a reaction product of a thiourethane resin precursor, etc. Commercially available thiourethane resin precursors include MR-7, MR-8, MR-10, and MR-174 manufactured by Mitsui Chemicals, Inc.

[0210] Examples of polyamide resins include aliphatic polyamide resins and aromatic polyamide resins. Examples of aliphatic polyamide resins include nylon 6, nylon 11, nylon 12, nylon 46, nylon 66, nylon 666, nylon 610, and nylon 612. Examples of aromatic polyamide resins include resins polymerized by dehydration condensation of diamines and dicarboxylic acids, in which at least one of the diamines and dicarboxylic acids contains an aromatic ring. Specific examples of aromatic polyamide resins include condensation polymers of metaxylylenediamine and adipic acid or adipic acid halide.

[0211] The resin may have an acid group. Examples of the acid group include a carboxy group, a phosphate group, a sulfonic acid group, and a phenolic hydroxy group. The acid group may be of one type or of two or more types. The resin having an acid group can be used as an alkali-soluble resin and can also be used as a dispersant.

[0212] For examples of resins having an acid group, see paragraphs

[0558] to

[0571] of JP 2012-208494 A (corresponding to paragraphs

[0685] to

[0700] of U.S. Patent Application Publication No. 2012 / 0235099 A) and paragraphs

[0076] to

[0099] of JP 2012-198408 A, the contents of which are incorporated herein by reference. Furthermore, as a resin having an acid group, ACRYBASE FF-426 (manufactured by Nippon Shokubai Co., Ltd.) can also be used.

[0213] The acid value of the resin having an acid group is preferably 30 to 200 mgKOH / g. The lower limit of the acid value is preferably 50 mgKOH / g or more, more preferably 70 mgKOH / g or more. The upper limit of the acid value is preferably 150 mgKOH / g or less, more preferably 120 mgKOH / g or less. The acid value of the resin is measured in accordance with JIS K0070 (1992) and calculated by converting 1 mmol / g = 56.1 mgKOH / g.

[0214] The resin may have a polymerizable group. Examples of the polymerizable group include an ethylenically unsaturated bond-containing group and a cyclic ether group. Examples of the ethylenically unsaturated bond-containing group include a vinyl group, a styrene group, an allyl group, a methallyl group, and a (meth)acryloyl group. Examples of the cyclic ether group include an epoxy group and an oxetanyl group.

[0215] Commercially available resins containing a polymerizable group include the Dianal BR series (polymethyl methacrylate (PMMA), such as Dianal BR-80, BR-83, and BR-87; manufactured by Mitsubishi Chemical Corporation), Photomer 6173 (a COOH-containing polyurethane acrylic oligomer; manufactured by Diamond Shamrock Co., Ltd.), Viscoat R-264, and KS Resist 106 (all manufactured by Osaka Organic Chemical Industry Ltd.), Cyclomer P series (e.g., ACA230AA), Plaxel CF200 series (all manufactured by Daicel Corporation), and Ebecryl 3800 (manufactured by Daicel-UCB Co., Ltd.), and Acrylicure RD-F8 (manufactured by Nippon Shokubai Co., Ltd.). Examples of commercially available resins include those described above for epoxy resins.

[0216] When the composition of the present invention is used for lenses (for example, eyeglass lenses), the resin is preferably a thermoplastic resin such as a carbonate resin or a (meth)acrylic resin, or a thermosetting resin such as a urethane resin.

[0217] A pressure-sensitive adhesive or adhesive can also be used for the resin. Examples of pressure-sensitive adhesives include acrylic pressure-sensitive adhesives, rubber pressure-sensitive adhesives, and silicone pressure-sensitive adhesives. An acrylic pressure-sensitive adhesive is a pressure-sensitive adhesive containing a polymer of a (meth)acrylic monomer ((meth)acrylic polymer). Examples of adhesives include urethane resin adhesives, polyester adhesives, acrylic resin adhesives, ethylene vinyl acetate resin adhesives, polyvinyl alcohol adhesives, polyamide adhesives, and silicone adhesives. Among these, urethane resin adhesives and silicone adhesives are preferred because of their high adhesive strength. Commercially available adhesives may be used, and examples of commercially available products include a urethane resin adhesive (LIS-073-50U: product name) from Toyo Ink Co., Ltd. and an acrylic pressure-sensitive adhesive (SK Dyne-SF2147: product name) from Soken Chemical & Engineering Co., Ltd.

[0218] The resin is preferably at least one selected from a (meth)acrylic resin, a polystyrene resin, a polyester resin, a polyurethane resin, a thiourethane resin, a polyimide resin, a polyamide resin, an epoxy resin, a polycarbonate resin, a phthalate resin, a cellulose acylate resin, and a cyclic olefin resin, and more preferably at least one selected from a (meth)acrylic resin, a polystyrene resin, a polyester resin, a polyurethane resin, and a cyclic olefin resin because they have good compatibility with the specific compound and are likely to produce a cured product with reduced surface unevenness.

[0219] The weight average molecular weight (Mw) of the resin is preferably 2,000 to 2,000,000. The lower limit of the Mw of the resin is preferably 5,000 or more, more preferably 10,000 or more, and even more preferably 50,000 or more. The upper limit of the Mw of the resin is preferably 1,000,000 or less, more preferably 500,000 or less, and even more preferably 200,000 or less. Furthermore, when an epoxy resin is used, the weight average molecular weight (Mw) of the epoxy resin is preferably 100 or more, more preferably 200 to 2,000,000. The upper limit of the Mw of the epoxy resin is preferably 1,000,000 or less, and more preferably 500,000 or less. The lower limit of the Mw of the epoxy resin is preferably 2,000 or more.

[0220] The weight average molecular weight (Mw) is a value measured by gel permeation chromatography (GPC). Measurement by GPC is performed using an HLC (registered trademark)-8020GPC (manufactured by Tosoh Corporation) as a measuring device, three TSKgel (registered trademark) Super Multipore HZ-H columns (4.6 mm ID x 15 cm, manufactured by Tosoh Corporation), and THF (tetrahydrofuran) as an eluent. The measurement conditions are a sample concentration of 0.45% by mass, a flow rate of 0.35 ml / min, a sample injection amount of 10 μl, and a measurement temperature of 40°C, and the measurement is performed using an RI detector. The calibration curve is prepared from eight samples of "Standard Sample TSK Standard, Polystyrene" from Tosoh Corporation: "F-40", "F-20", "F-4", "F-1", "A-5000", "A-2500", "A-1000", and "n-propylbenzene".

[0221] The total light transmittance of the resin is preferably 80% or more, more preferably 85% or more, and even more preferably 90% or more. In this specification, the total light transmittance of the resin is a value measured based on the contents described on pages 225-232 of "4th Edition Experimental Chemistry Lectures 29: Polymer Material Media" (Maruzen, 1992), edited by the Chemical Society of Japan.

[0222] The content of the curable compound in the total solid content of the composition is preferably 1 to 99.9% by mass. The lower limit is preferably 30% by mass or more, more preferably 50% by mass or more, and even more preferably 70% by mass or more. The upper limit is preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 80% by mass or less. The composition may contain only one type of curable compound, or may contain two or more types. When two or more types of curable compounds are contained, the total amount thereof is preferably within the above range.

[0223] When the curable compound contained in the composition of the present invention contains a resin, the content of the resin in the total solid content of the composition is preferably 1 to 99.9% by mass. The lower limit is preferably 30% by mass or more, more preferably 50% by mass or more, and even more preferably 70% by mass or more. The upper limit is preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 80% by mass or less. The composition may contain only one type of resin, or may contain two or more types. When two or more types of resins are contained, the total amount thereof is preferably within the above range.

[0224] When the curable compound contained in the composition of the present invention includes a polymerizable compound, the content of the polymerizable compound in the total solid content of the composition is preferably 0.1 to 90% by mass. The lower limit is preferably 1% by mass or more, and more preferably 5% by mass or more. The upper limit is preferably 80% by mass or less, and more preferably 70% by mass or less. The composition of the present invention may contain only one type of polymerizable compound, or may contain two or more types. When two or more types of polymerizable compounds are contained, the total amount thereof is preferably within the above range.

[0225] <<Polymerization Initiator>> The composition of the present invention may contain a polymerization initiator. The polymerization initiator may be a compound capable of generating an initiating species necessary for a polymerization reaction upon application of energy. Examples of the polymerization initiator include radical polymerization initiators and cationic polymerization initiators. When a radically polymerizable compound is used as the polymerizable compound, the polymerization initiator is preferably a radical polymerization initiator. When a cationic polymerizable compound is used as the polymerizable compound, the polymerization initiator is preferably a cationic polymerization initiator. The polymerization initiator may be appropriately selected from, for example, photopolymerization initiators and thermal polymerization initiators, with photopolymerization initiators being preferred. The photopolymerization initiator is a compound that is photosensitive to exposure light and initiates or promotes polymerization of the polymerizable compound. Examples of the photopolymerization initiator include photoradical polymerization initiators and photocationic polymerization initiators, with photoradical polymerization initiators being preferred. The photoradical polymerization initiator is preferably a compound that generates radicals in response to actinic rays with a wavelength of 300 nm or more.

[0226] (Photoradical Polymerization Initiator) Examples of the photoradical polymerization initiator include oxime compounds, halogenated hydrocarbon derivatives (for example, compounds having a triazine skeleton, compounds having an oxadiazole skeleton, etc.), oxydiazole compounds, carbonyl compounds, ketal compounds, benzoin compounds, acridine compounds, organic peroxides, azo compounds, coumarin compounds, azide compounds, metallocene compounds, hexaarylbiimidazole compounds, organic boric acid compounds, disulfonic acid compounds, onium salt compounds, acetophenone compounds, acylphosphine compounds, and benzophenone compounds.

[0227] Examples of acetophenone compounds include aminoacetophenone compounds and hydroxyacetophenone compounds. Examples of acetophenone compounds include the acetophenone compounds described in JP-A-2009-191179 and JP-A-10-291969. Commercially available aminoacetophenone compounds include Omnirad 907, Omnirad 369, Omnirad 369E, and Omnirad 379EG (all manufactured by IGM Resins B.V.). Commercially available hydroxyacetophenone compounds include Omnirad 184, Omnirad 1173, Omnirad 2959, and Omnirad 127 (all manufactured by IGM Resins B.V.).

[0228] Examples of the acylphosphine compound include the acylphosphine compounds described in Japanese Patent No. 4225898. Examples of commercially available acylphosphine compounds include Omnirad 819 and Omnirad TPO (both manufactured by IGM Resins B.V.).

[0229] The benzophenone compound includes benzophenone, 2-methylbenzophenone, 3-methylbenzophenone, 4-methylbenzophenone, 4-methoxybenzophenone, 2-chlorobenzophenone, 4-chlorobenzophenone, 4-bromobenzophenone, 2-carboxybenzophenone, 2-ethoxycarbonylbenzophenone, benzophenonetetracarboxylic acid or its tetramethyl ester, 4,4'-bis(dialkylamino)benzophenones (e.g., 4,4'-bis(dimethylamino)benzophenone, 4,4'-bis(dicyclohexylamino)benzophenone, 4,4'-bis(diethylamino)benzophenone, 4,4'-bis(dihydroxyethylamino)benzophenone), 4-methoxy-4'-dimethylaminobenzophenone, 4,4'-dimethoxybenzophenone, 4-dimethylaminobenzophenone, 4-dimethylaminoacetophenone, and the like. From the viewpoint of sensitivity and light resistance of the resulting cured product, 4,4'-bis(diethylamino)benzophenone is preferred.

[0230] Examples of oxime compounds include the compounds described in JP-A-2001-233842, JP-A-2000-080068, JP-A-2006-342166, and JP-A-2016-006475, paragraphs 0073 to 0075. Among the oxime compounds, oxime ester compounds are preferred. Commercially available oxime compounds include Irgacure OXE01, Irgacure OXE02 (manufactured by BASF), and Irgacure OXE03 (manufactured by BASF).

[0231] Examples of halogenated hydrocarbon derivatives include those described in Wakabayashi et al., Bull Chem. Soc. Japan, 42, 2924 (1969), U.S. Pat. No. 3,905,815, JP-B No. 46-004605, JP-A No. 48-036281, JP-A No. 55-032070, JP-A No. 60-239736, JP-A No. 61-169835, JP-A No. 61-169837, JP-A No. 62-058241, JP-A No. 62-212401, JP-A No. 63-070243, JP-A No. 63-298339, M.P. Examples of such compounds include those described in Hutt, Journal of Heterocyclic Chemistry, 1 (No. 3), (1970), and are preferably oxazole compounds or triazine compounds substituted with a trihalomethyl group.

[0232] Examples of the hexaarylbiimidazole compound include compounds described in Japanese Patent Publication No. 06-029285, U.S. Pat. Nos. 3,479,185, 4,311,783, and 4,622,286. Specific examples include 2,2'-bis(o-chlorophenyl)-4,4',5,5'-tetraphenylbiimidazole, 2,2'-bis(o-bromophenyl)-4,4',5,5'-tetraphenylbiimidazole, 2,2'-bis(o,p-dichlorophenyl)-4,4',5,5'-tetraphenylbiimidazole, and 2,2'-bis(o-chlorophenyl)-4,4',5,5'-tetra(m-methoxyphenyl)biimidazole. 2,2'-bis(o,o'-dichlorophenyl)-4,4',5,5'-tetraphenylbiimidazole, 2,2'-bis(o-nitrophenyl)-4,4',5,5'-tetraphenylbiimidazole, 2,2'-bis(o-methylphenyl)-4,4',5,5'-tetraphenylbiimidazole, 2,2'-bis(o-trifluorophenyl)-4,4',5,5'-tetraphenylbiimidazole, and the like.

[0233] (Photocationic Polymerization Initiator) The photocationic polymerization initiator is not particularly limited as long as it is a compound that generates a protonic acid or a Lewis acid upon irradiation with light. The photoacid generator is preferably a compound that responds to actinic rays with a wavelength of 300 nm or more, more preferably 300 to 450 nm, and generates an acid. The photoacid generator is preferably a compound that generates an acid having a pKa of 4 or less upon irradiation with light, more preferably a compound that generates an acid having a pKa of 3 or less, and even more preferably a compound that generates an acid having a pKa of 2 or less.

[0234] Examples of the photocationic polymerization initiator include oxime sulfonate compounds, triazine compounds, sulfonium salts, iodonium salts, quaternary ammonium salts, diazomethane compounds, sulfone compounds, sulfonic acid ester compounds, iminosulfonic acid ester compounds, carboxylic acid ester compounds, and sulfonimide compounds.

[0235] Specific examples of the photocationic polymerization initiator include the compounds described in paragraphs 0061 to 0108 of JP-A 2012-046577 and 0029 to 0030 of JP-A 2002-122994, the compounds described in paragraphs 0037 to 0063 of JP-A 2002-122994, and the oxime sulfonate compounds described in paragraphs 0081 to 0108 of JP-A 2013-210616. Commercially available photocationic polymerization initiators include WPAG-469 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), CPI-100P (manufactured by San-Apro Co., Ltd.), CPI-210S (manufactured by San-Apro Co., Ltd.), and Irgacure 290 (BASF Japan Ltd.).

[0236] (Thermal Polymerization Initiator) The thermal polymerization initiator is not particularly limited, and known thermal polymerization initiators can be used. For example, azo compounds such as 2,2'-azobis(isobutyrate)dimethyl, 2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethyl-4-methoxyvaleronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), dimethyl-2,2'-azobis(2-methylpropionate), 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis(N-butyl-2-methylpropionamide), dimethyl 1,1'-azobis(1-cyclohexanecarboxylate), and 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride; Examples of the peroxide include organic peroxides such as 1,1-di(t-hexylperoxy)cyclohexane, 1,1-di(t-butylperoxy)cyclohexane, 2,2-di(4,4-di-(t-butylperoxy)cyclohexyl)propane, t-hexylperoxyisopropyl monocarbonate, t-butylperoxy-3,5,5-trimethylhexanoate, t-butylperoxylaurate, dicumyl peroxide, di-t-butyl peroxide, t-butylperoxy-2-ethylhexanoate, t-hexylperoxy-2-ethylhexanoate, cumene hydroperoxide, and t-butyl hydroperoxide; and inorganic peroxides such as potassium persulfate, ammonium persulfate, and hydrogen peroxide.

[0237] When the composition of the present invention contains a polymerization initiator, the content of the polymerization initiator in the total solid content of the composition is preferably 0.1 to 20% by mass. The lower limit is preferably 0.3% by mass or more, and more preferably 0.4% by mass or more. The upper limit is preferably 15% by mass or less, and more preferably 10% by mass or less. The composition of the present invention may contain only one type of polymerization initiator, or may contain two or more types. When two or more types of polymerization initiators are contained, the total amount thereof is preferably within the above range.

[0238] <<Catalyst>> The composition of the present invention can contain a catalyst. Examples of the catalyst include acid catalysts such as hydrochloric acid, sulfuric acid, acetic acid, and propionic acid, and base catalysts such as sodium hydroxide, potassium hydroxide, and triethylamine. When the composition of the present invention contains a catalyst, the content of the catalyst is preferably 0.1 to 100 parts by mass, more preferably 0.1 to 50 parts by mass, and even more preferably 0.1 to 20 parts by mass, per 100 parts by mass of the resin. The composition of the present invention may contain only one type of catalyst, or may contain two or more types. When two or more types of catalysts are contained, the total amount thereof preferably falls within the above range.

[0239] <<Silane Coupling Agent>> The composition of the present invention can contain a silane coupling agent. According to this embodiment, the adhesion of the resulting film to the support can be further improved. In the present invention, the silane coupling agent refers to a silane compound having a hydrolyzable group and other functional groups. The hydrolyzable group refers to a substituent directly bonded to a silicon atom that can form a siloxane bond through at least one of a hydrolysis reaction and a condensation reaction. Examples of the hydrolyzable group include a halogen atom, an alkoxy group, and an acyloxy group, with an alkoxy group being preferred. That is, the silane coupling agent is preferably a compound having an alkoxysilyl group. Examples of functional groups other than the hydrolyzable group include a vinyl group, a (meth)allyl group, a (meth)acryloyl group, a mercapto group, an epoxy group, an oxetanyl group, an amino group, a ureido group, a sulfide group, an isocyanate group, and a phenyl group, with an amino group, a (meth)acryloyl group, and an epoxy group being preferred. Specific examples of silane coupling agents include the compounds described in paragraphs 0018 to 0036 of JP 2009-288703 A and the compounds described in paragraphs 0056 to 0066 of JP 2009-242604 A, the contents of which are incorporated herein by reference. Commercially available silane coupling agents include A-50 (organosilane) from Soken Chemical & Engineering Co., Ltd. The content of the silane coupling agent in the total solids content of the composition of the present invention is preferably 0.1 to 5% by mass. The upper limit is preferably 3% by mass or less, more preferably 2% by mass or less. The lower limit is preferably 0.5% by mass or more, more preferably 1% by mass or more. The silane coupling agent may be used alone or in combination with two or more types. When two or more types are used, it is preferable that the total amount is within the above range.

[0240] <<Surfactant>> The composition of the present invention may contain a surfactant. Examples of the surfactant include those described in paragraph 0017 of Japanese Patent No. 4,502,784 and paragraphs 0060 to 0071 of JP-A-2009-237362.

[0241] The surfactant is preferably a nonionic surfactant, a fluorine-based surfactant, or a silicone-based surfactant.

[0242] Commercially available fluorine-based surfactants include Megafac F-171, F-172, F-173, F-176, F-177, F-141, F-142, F-143, F-144, F-437, F-475, F-477, F-479, F-482, F-551-A, F-552, F-554, F-555-A, F-556, F-557, F-558, F-559, and F-5 60, F-561, F-565, F-563, F-568, F-575, F-780, EXP, MFS-330, R-41, R-41-LM, R-01, R-40, R-40-LM, RS-43, TF-1956, RS-90, R-94, RS-72-K, DS-21 (all manufactured by DIC Corporation), Fluorad FC430, FC431, FC171 (all manufactured by Sumitomo 3M Limited), Surflon S-382, SC-101, SC-103, SC-104, SC-105, SC-1068, SC-381, SC-383, S-393, KH-40 (all manufactured by AGC Inc.), PolyFox PF636, PF656, PF6320, PF6520, PF7002 (all manufactured by OMNOVA), Ftergent Examples include 710FM, 610FM, 601AD, 601ADH2, 602A, 215M, 245F, 251, 212M, 250, 209F, 222F, 208G, 710LA, 710FS, 730LM, 650AC, and 681 (all manufactured by NEOS Corporation).

[0243] As the fluorosurfactant, an acrylic compound having a molecular structure with a functional group containing a fluorine atom, which cleaves the functional group when heated, causing the fluorine atom to volatilize, can also be suitably used. Examples of such fluorosurfactants include the Megafac DS series manufactured by DIC Corporation (The Chemical Daily (February 22, 2016), The Nikkei Business Daily (February 23, 2016)), such as Megafac DS-21.

[0244] As the fluorine-based surfactant, it is also preferable to use a polymer of a fluorine atom-containing vinyl ether compound having a fluorinated alkyl group or a fluorinated alkylene ether group and a hydrophilic vinyl ether compound.

[0245] The fluorine-based surfactant may also be a block polymer.

[0246] As the fluorine-based surfactant, a fluorine-containing polymer compound containing a repeating unit derived from a (meth)acrylate compound having a fluorine atom and a repeating unit derived from a (meth)acrylate compound having two or more (preferably five or more) alkyleneoxy groups (preferably ethyleneoxy groups or propyleneoxy groups) can also be used.

[0247] The fluorine-containing surfactant may also be a fluorine-containing polymer having an ethylenically unsaturated bond-containing group in the side chain. Commercially available products include Megafac RS-101, RS-102, RS-718K, and RS-72-K (all manufactured by DIC Corporation).

[0248] Furthermore, since there are concerns about the environmental compatibility of compounds having a linear perfluoroalkyl group having seven or more carbon atoms, it is preferable to use a fluorosurfactant that uses an alternative material to perfluorooctanoic acid (PFOA) or perfluorooctanesulfonic acid (PFOS).

[0249] Examples of silicone surfactants include linear polymers formed from siloxane bonds and modified siloxane polymers having organic groups introduced into the side chains or terminals. Commercially available silicone surfactants include DOWSIL 8032 ADDITIVE, Toray Silicone DC3PA, Toray Silicone SH7PA, Toray Silicone DC11PA, Toray Silicone SH21PA, Toray Silicone SH28PA, Toray Silicone SH29PA, Toray Silicone SH30PA, and Toray Silicone SH8400 (all manufactured by Dow Corning Toray Co., Ltd.), X-22-4952, X-22-4272, X-22-6266, KF-351A, K354L, KF-355A, and KF-94. No. 5, KF-640, KF-642, KF-643, X-22-6191, X-22-4515, KF-6004, KP-341, KF-6001, KF-6002 (all manufactured by Shin-Etsu Silicones Co., Ltd.), F-4440, TSF-4300, TSF-4445, TSF-4460, TSF-4452 (all manufactured by Momentive Performance Materials), BYK307, BYK323, BYK330 (all manufactured by BYK-Chemie).

[0250] Examples of nonionic surfactants include glycerol, trimethylolpropane, trimethylolethane, and their ethoxylates and propoxylates (for example, glycerol propoxylate, glycerol ethoxylate, etc.), polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene oleyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene nonylphenyl ether, polyethylene glycol dilaurate, polyethylene glycol distearate, and sorbitan fatty acid esters. Commercially available nonionic surfactants include Pluronic L10, L31, L61, L62, 10R5, 17R2, and 25R2 (manufactured by BASF), Tetronic 304, 701, 704, 901, 904, and 150R1 (manufactured by BASF), Solsperse 20000 (manufactured by Lubrizol Nippon Co., Ltd.), NCW-101, NCW-1001, and NCW-1002 (manufactured by Fujifilm Wako Pure Chemical Industries Co., Ltd.), Paionin D-6112, D-6112-W, and D-6315 (manufactured by Takemoto Oil & Fat Co., Ltd.), and Olfine E1010 and Surfynol 104, 400, and 440 (manufactured by Nissin Chemical Industry Co., Ltd.).

[0251] The content of the surfactant in the total solid content of the composition of the present invention is preferably 0.01 to 3.0 mass%, more preferably 0.05 to 1.0 mass%, and even more preferably 0.10 to 0.80 mass%. The surfactant may be one type or two or more types. When two or more types are used, it is preferable that the total amount is in the above range.

[0252] <<Solvent>> The composition of the present invention preferably further contains a solvent. The solvent is not particularly limited, and examples thereof include water and organic solvents. The solvent is preferably an organic solvent.

[0253] Examples of organic solvents include alcohol-based solvents, ester-based solvents, ether-based solvents, ketone-based solvents, amide-based solvents, hydrocarbon-based solvents, halogen-based solvents, etc. Specific examples of alcohol-based solvents include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 2-methyl-1-propanol, 1-methoxy-2-propanol, 2-ethoxyethanol, 2-butoxyethanol, ethylene glycol, propylene glycol, and glycerin. Specific examples of ester solvents include methyl acetate, ethyl acetate, n-butyl acetate, isobutyl acetate, amyl formate, isoamyl acetate, isobutyl acetate, butyl propionate, isopropyl butyrate, ethyl butyrate, butyl butyrate, methyl lactate, ethyl lactate, alkoxyacetic acid alkyl esters (e.g., methyl alkoxyacetate, ethyl alkoxyacetate, butyl alkoxyacetate (specifically, methyl methoxyacetate, ethyl methoxyacetate, butyl methoxyacetate, methyl ethoxyacetate, ethyl ethoxyacetate, etc.)), 3-oxypropionic acid alkyl esters, and 2-oxypropionic acid alkyl esters. , methyl 2-oxy-2-methylpropionate, ethyl 2-oxy-2-methylpropionate, methyl pyruvate, ethyl pyruvate, propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, methyl 2-oxobutanoate, ethyl 2-oxobutanoate, methyl cellosolve acetate, ethyl cellosolve acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, ethylene carbonate, and the like.Specific examples of ether-based solvents include diethylene glycol dimethyl ether, tetrahydrofuran, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, polyethylene glycol monoalkyl ether, polypropylene glycol monoalkyl ether, polyethylene glycol, polypropylene glycol, ethylene glycol dialkyl ether, propylene glycol dialkyl ether, polyethylene glycol dialkyl ether, polypropylene glycol dialkyl ether, and dioxane. Specific examples of amide-based solvents include N-methylpyrrolidone, dimethylformamide, and dimethylacetamide. Specific examples of ketone-based solvents include methyl ethyl ketone, cyclohexanone, cyclopentanone, 2-heptanone, and 3-heptanone. Specific examples of hydrocarbon-based solvents include toluene and xylene. Specific examples of halogen-based solvents include chloroform and methylene chloride. Two or more of these organic solvents may be used in combination.

[0254] The organic solvent preferably contains at least one selected from methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, ethyl cellosolve acetate, ethyl lactate, diethylene glycol dimethyl ether, butyl acetate, methyl 3-methoxypropionate, 2-heptanone, cyclohexanone, cyclopentanone, ethyl carbitol acetate, butyl carbitol acetate, propylene glycol monomethyl ether, and propylene glycol monomethyl ether acetate.

[0255] The content of the solvent in the composition of the present invention is preferably 10 to 90% by mass, more preferably 30 to 90% by mass, and even more preferably 50 to 90% by mass. The composition of the present invention may contain only one solvent, or may contain two or more solvents. When two or more solvents are contained, the total amount thereof is preferably within the above range. Furthermore, when the composition of the present invention is used as a kneaded product, the content of the organic solvent in the composition is preferably 0.1% by mass or less, and more preferably 0.01% by mass or less.

[0256] <<Plasticizer>> When the composition of the present invention is used as a kneaded product, the composition of the present invention may contain a plasticizer. Examples of the plasticizer include phthalate ester-based plasticizers, phosphate ester-based plasticizers, trimellitate ester-based plasticizers, fatty acid ester-based plasticizers, polyester-based plasticizers, glycerin-based plasticizers, and polyalkylene glycol-based plasticizers, with phthalate ester-based plasticizers and phosphate ester-based plasticizers being preferred.

[0257] Examples of phthalate ester plasticizers include dimethyl phthalate, diethyl phthalate, diisopropyl phthalate, dibutyl phthalate, diisobutyl phthalate, dihexyl phthalate, dicyclohexyl phthalate, diphenyl phthalate, bis(2-ethylhexyl) phthalate, diisononyl phthalate, diisodecyl phthalate, and diundecyl phthalate. Examples of phosphate ester plasticizers include trimethyl phosphate, triethyl phosphate, tributyl phosphate, triphenyl phosphate, and tricresyl phosphate. Examples of trimellitate ester plasticizers include tributyl trimellitate and tris(2-ethylhexyl) trimellitate. Examples of fatty acid ester plasticizers include dimethyl adipate, diethyl adipate, dipropyl adipate, diisopropyl adipate, dibutyl adipate, diisobutyl adipate, dimethyl dodecanoate, dibutyl maleate, and ethyl oleate. Examples of polyester-based plasticizers include polyesters composed of an acid component such as adipic acid, sebacic acid, terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, diphenyldicarboxylic acid, or rosin, and a diol component such as propylene glycol, 1,3-butanediol, 1,4-butanediol, 1,6-hexanediol, ethylene glycol, or diethylene glycol, as well as polyesters with hydroxycarboxylic acids such as polycaprolactone. These polyesters may be end-capped with a monofunctional carboxylic acid or a monofunctional alcohol, or may be end-capped with an epoxy compound or the like. Examples of glycerin-based plasticizers include glycerin monoacetomonolaurate, glycerin diacetomonolaurate, glycerin monoacetomonostearate, glycerin diacetomonooleate, and glycerin monoacetomonomonoacetate.Examples of the polyalkylene glycol plasticizer include polyalkylene glycols such as polyethylene glycol, polypropylene glycol, polytetramethylene glycol, ethylene oxide addition polymers of bisphenols, propylene oxide addition polymers of bisphenols, and tetrahydrofuran addition polymers of bisphenols, as well as terminal epoxy-modified compounds, terminal ester-modified compounds, and terminal ether-modified compounds thereof.

[0258] The molecular weight of the plasticizer is preferably less than 3,000, more preferably 2,000 or less, and even more preferably 1,500 or less.

[0259] The content of the plasticizer in the composition of the present invention is preferably 0.001 to 30% by mass. The lower limit is preferably 0.005% by mass or more, and more preferably 0.01% by mass or more. The upper limit is preferably 20% by mass or less, and more preferably 10% by mass or less. The kneaded product may contain only one type of plasticizer, or may contain two or more types. When two or more types of plasticizers are contained, the total amount thereof is preferably within the above range.

[0260] <<Other Additives>> The composition of the present invention may contain, as necessary, any additives such as a processing stabilizer, an antioxidant, a compatibilizer, etc. By adding these components as needed, various properties of the resulting cured product can be adjusted appropriately.

[0261] <Uses of Composition> The composition of the present invention can also be suitably used in applications where it may be exposed to sunlight or light including ultraviolet rays.Specific examples include coating materials or films for window glass of residences, facilities, transportation equipment, etc.; interior and exterior materials and interior and exterior paints for residences, facilities, transportation equipment, etc.; light source components that emit ultraviolet rays, such as fluorescent lamps and mercury lamps; components for solar cells, precision machinery, electronic and electrical equipment, and display devices; containers or packaging materials for food, chemicals, medicines, etc.; agricultural and industrial sheets; textile products and fibers for clothing, such as sportswear, stockings, and hats; lenses or coating materials thereof, such as plastic lenses, contact lenses, glasses, and artificial eyes; optical products, such as optical filters, prisms, mirrors, and photographic materials; stationery, such as tapes and inks; sign plates, markers, etc., and surface coating materials thereof. For details of these, please refer to paragraphs 0158 to 0218 of JP-A-2009-263617 and paragraphs 0161 to 0194 of JP-A-2009-096971, the contents of which are incorporated herein by reference.

[0262] The composition of the present invention can be preferably used for optical components, etc. For example, it is preferably used as a composition for ultraviolet cut filters, lenses, or protective materials. The form of the protective material is not particularly limited, but examples include a coating film, a film, and a sheet. The composition of the present invention can also be used as a pressure-sensitive adhesive or an adhesive.

[0263] The composition of the present invention can also be used in various components of display devices. For example, in the case of a liquid crystal display device, the composition can be used in components constituting the liquid crystal display device, such as an antireflection film, a polarizing plate protective film, an optical film, a retardation film, a pressure-sensitive adhesive, and an adhesive. In the case of an organic electroluminescence display device, the composition can be used in components constituting the organic electroluminescence display device, such as an optical film, a polarizing plate protective film in a circular polarizing plate, a retardation film such as a quarter-wave plate, an adhesive, or a pressure-sensitive adhesive.

[0264] <Cured Product and Applications Thereof> The cured product of the present invention is obtained using the composition of the present invention described above. In this specification, the term "cured product" includes a dried product obtained by drying and solidifying the composition, and, in the case where the composition undergoes a curing reaction, a cured product obtained by curing the composition.

[0265] The cured product of the present invention may be obtained as a molded article obtained by molding the composition into a desired shape. The shape of the molded article can be appropriately selected depending on the application and purpose. Examples of the shape of the molded article include a coating film, a film, a sheet, a plate, a lens, a tube, and a fiber.

[0266] The cured product of the present invention is preferably used as an optical element, such as an ultraviolet cut filter, a lens, or a protective material. It can also be used as a polarizing plate.

[0267] The ultraviolet cut filter can be used in products such as optical filters, display devices, solar cells, window glass, etc. The type of display device is not particularly limited, but examples include liquid crystal display devices and organic electroluminescence display devices.

[0268] When the cured product of the present invention is used for a lens, the cured product of the present invention itself may be formed into a lens shape and used. The cured product of the present invention may also be used as a coating film on a lens surface or as an intermediate layer (adhesive layer) of a cemented lens. Examples of cemented lenses include those described in paragraphs 0094 to 0102 of WO 2019 / 131572, the contents of which are incorporated herein by reference.

[0269] The type of protective material is not particularly limited, but examples thereof include protective materials for display devices, protective materials for solar cells, protective materials for window glass, organic electroluminescence display devices, etc. The shape of the protective material is not particularly limited, but examples thereof include coating film, film, sheet, etc.

[0270] <Optical Element> The optical element of the present invention includes a cured product obtained using the composition of the present invention described above. The cured product of the present invention may be obtained as a molded product obtained by molding the composition of the present invention described above into a desired shape. The shape of the molded product can be appropriately selected depending on the application and purpose. Examples include a coating film, film, sheet, plate, lens, tube, fiber, etc.

[0271] The optical members include ultraviolet cut filters, lenses, and protective materials.

[0272] The ultraviolet cut filter can be used in products such as optical filters, display devices, solar cells, window glass, etc. The type of display device is not particularly limited, but examples include liquid crystal display devices and organic electroluminescence display devices.

[0273] Examples of lenses include those in which the cured product of the present invention itself is formed into a lens shape; and those in which the cured product of the present invention is used as a coating film on the surface of a lens or as an intermediate layer (adhesive layer or pressure-sensitive adhesive layer) of a cemented lens.

[0274] The type of protective material is not particularly limited, but examples thereof include protective materials for display devices, protective materials for solar cells, protective materials for window glass, etc. The shape of the protective material is not particularly limited, but examples thereof include coating film, film, sheet, etc.

[0275] Another example of an optical component is a resin film. Resin films can be formed using the composition of the present invention, which uses a resin as the curable compound. Resins used in resin film-forming compositions include the resins described above, with (meth)acrylic resins, polyester fibers, cyclic olefin resins, and cellulose acylate resins being preferred, and cellulose acylate resins being more preferred. Resin film-forming compositions can contain additives described in paragraphs 0022 to 0067 of JP 2012-215689 A. Examples of such additives include sugar esters. Adding a sugar ester compound to a resin film-forming composition containing a cellulose acylate resin can reduce total haze and internal haze without impairing the expression of optical properties and even without heat treatment before the stretching process. Furthermore, resin films (cellulose acylate films) using compositions containing a cellulose acylate resin can be produced by the method described in paragraphs 0068 to 0096 of JP 2012-215689 A. The resin film may further be laminated with a hard coat layer described in paragraphs 0097 to 0113 of JP-A-2012-215689.

[0276] Another example of an optical member is an optical member having a laminate of a support and a resin layer, in which at least one of the support and the resin layer contains the cured product of the present invention.

[0277] The thickness of the resin layer in the laminate is preferably 1 μm to 2500 μm, and more preferably 10 μm to 500 μm.

[0278] The support in the laminate is preferably a material having transparency to the extent that the optical performance is not impaired. The support being transparent means that the support is optically transparent, specifically, the support has a total light transmittance of 85% or more. The total light transmittance of the support is preferably 90% or more, more preferably 95% or more.

[0279] A suitable example of the support is a resin film. Examples of resins constituting the resin film include ester resins (e.g., polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), polycyclohexanedimethylene terephthalate (PCT)), olefin resins (e.g., polypropylene (PP), polyethylene (PE)), polyvinyl chloride (PVA), tricellulose acetate (TAC), etc. Among these, PET is preferred in terms of versatility.

[0280] The thickness of the support can be appropriately selected depending on the application or purpose, etc. In general, the thickness is preferably 5 μm to 2500 μm, and more preferably 20 μm to 500 μm.

[0281] The support may also be a releasable support. Such a laminate is preferably used for a polarizing plate or the like. Here, the releasable support refers to a support that can be peeled off from the resin film. The stress when peeling the support from the resin film is preferably 0.05 N / 25 mm or more and 2.00 N / 25 mm or less, more preferably 0.08 N / 25 mm or more and 0.50 N / 25 mm or less, and even more preferably 0.11 N / 25 mm or more and 0.20 N / 25 mm or less. The stress when peeling the support from the resin film was evaluated by first pasting and fixing the surface of the laminate cut to a width of 25 mm and a length of 80 mm to a glass substrate via an acrylic pressure-sensitive adhesive sheet, and then using a tensile tester (RTF-1210 manufactured by A&D Co., Ltd.), one end of the length direction of the test piece (one side of the 25 mm width) was gripped and a 90° peel test (in accordance with Japanese Industrial Standards (JIS) K 6854-1:1999 "Adhesives - Test method for peel adhesion strength - Part 1: 90° peel") was carried out at a temperature of 23°C and a relative humidity of 60% at a crosshead speed (grip movement speed) of 200 mm / min.

[0282] The release support preferably contains polyethylene terephthalate (PET) as the main component (the component with the highest mass content among the components constituting the support). From the viewpoint of mechanical strength, the weight-average molecular weight of PET is preferably 20,000 or more, more preferably 30,000 or more, and even more preferably 40,000 or more. The weight-average molecular weight of PET can be determined by dissolving the support in hexafluoroisopropanol (HFIP) and using the GPC method described above. The thickness of the support is not particularly limited, but is preferably 0.1 to 100 μm, more preferably 0.1 to 75 μm, even more preferably 0.1 to 55 μm, and particularly preferably 0.1 to 10 μm. The support may also be subjected to known surface treatments such as corona treatment, glow discharge treatment, and undercoating.

[0283] Another example of an optical component is a laminate having a hard coat layer, a transparent support, and a pressure-sensitive adhesive layer or adhesive layer laminated in this order. Such a laminate is preferably used as an ultraviolet cut filter or a protective material (protective film, protective sheet). In this optical component, any of the support, the hard coat layer, and the pressure-sensitive adhesive layer or adhesive layer may contain the cured product of the present invention.

[0284] Examples of hard coat layers include those described in JP 2013-045045 A, JP 2013-043352 A, JP 2012-232459 A, JP 2012-128157 A, JP 2011-131409 A, JP 2011-131404 A, JP 2011-126162 A, JP 2011-075705 A, JP 2009-286981 A, JP 2009-263567 A, and JP 2009 The hard coat layer described in JP-A-075248, JP-A-2007-164206, JP-A-2006-096811, JP-A-2004-075970, JP-A-2002-156505, JP-A-2001-272503, WO 2012 / 018087, WO 2012 / 098967, WO 2012 / 086659, and WO 2011 / 105594 can be applied. The thickness of the hard coat layer is preferably 5 to 100 μm in order to further improve scratch resistance.

[0285] This optical component has a pressure-sensitive adhesive layer or adhesive layer on the side of the supporting substrate opposite the side having the hard coat layer. The type of pressure-sensitive adhesive or adhesive used in the pressure-sensitive adhesive layer or adhesive layer is not particularly limited, and known pressure-sensitive adhesives or adhesives can be used. It is also preferable to use a pressure-sensitive adhesive or adhesive containing an acrylic resin described in paragraphs 0056 to 0076 of JP 2017-142412 A and a crosslinking agent described in paragraphs 0077 to 0082 of JP 2017-142412 A. The pressure-sensitive adhesive or adhesive may also contain an adhesion improver (silane compound) described in paragraphs 0088 to 0097 of JP 2017-142412 A, and an additive described in paragraph 0098 of JP 2017-142412 A. The pressure-sensitive adhesive or adhesive layer can be formed by the method described in paragraphs 0099 to 0100 of JP 2017-142412 A. The thickness of the adhesive layer or the bonding layer is preferably 5 μm to 100 μm in terms of achieving both adhesive strength and ease of handling.

[0286] The optical member of the present invention can be preferably used as a component of a display such as a liquid crystal display device (LCD) or an organic electroluminescence display device (OLED).

[0287] Examples of liquid crystal display devices include those containing the cured product of the present invention in components such as antireflection films, polarizing plate protective films, optical films, retardation films, pressure-sensitive adhesives, adhesives, etc. Optical components containing the cured product of the present invention may be placed on either the viewer side (front side) or the backlight side of the liquid crystal cell, and may also be placed on either the side of the polarizer farther from the liquid crystal cell (outer side) or the side close to the liquid crystal cell (inner side).

[0288] Examples of organic electroluminescent display devices include those containing the cured product of the present invention in components such as optical films, polarizer protective films in circular polarizers, retardation films such as quarter-wave plates, adhesives, pressure-sensitive adhesives, etc. By using the cured product of the present invention in the above configuration, deterioration of the organic electroluminescent display device due to external light can be suppressed.

[0289] The present invention will be explained in more detail below with reference to examples. The materials, amounts used, ratios, treatment details, treatment procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the specific examples shown below. In addition, in the structural formula shown below, Me is a methyl group, Et is an ethyl group, n Bu is a normal butyl group, t Bu is a tert-butyl group and Ph is a phenyl group.

[0290] <Synthesis Examples> (Synthesis Example 1) Synthesis of Intermediate 1-3 Intermediate 1-1 was synthesized according to the following scheme: In the following scheme, intermediate 1-1 was synthesized with reference to the method described in paragraphs

[0222] and

[0223] of JP 2009-263617 A, using 1,2-dibenzylpyrazolidine-3,5-dione instead of 1,2-dibutylpyrazolidine-3,5-dione, to obtain 77 g of intermediate 1-1 (yield: 78%).

[0291] Next, intermediate 1-2 was synthesized according to the following synthesis scheme. 50 g of intermediate 1-1, 24.5 g of 2,3-dichloro-5,6-dicyano-p-benzoquinone, and 500 ml of tetrahydrofuran were mixed together and stirred at 20°C for 1 hour. After completion of the reaction, 500 mL of hexane was added, and the precipitated solid was collected by filtration and washed with 150 ml of hexane, yielding 42 g of intermediate 1-2 (yield 84%).

[0292] Next, intermediate 1-3 was synthesized according to the following synthesis scheme. 30 g of intermediate 1-2, 8 g of piperidinium pentamethylenedithiocarbamate, 360 mL of N-methyl-2-pyrrolidone, 160 mL of acetic acid, and 54 mL of acetone were mixed and stirred at 60° C. for 1 hour. The precipitated solid was collected by filtration and washed with 300 mL of acetone, yielding 8.0 g of intermediate 1-3 (yield 36%).

[0293] (Synthesis Example 2) Synthesis of Compound A-104 Compound A-104 was synthesized according to the following synthesis scheme. 3.0 g of intermediate 1-3, 0.58 g of malononitrile, and 150 ml of N-methyl-2-pyrrolidone were mixed and stirred at 80°C for 1 hour. After cooling to room temperature, 1 mL of hydrochloric acid and 150 ml of water were added and stirred for 30 minutes. The precipitated solid was collected by filtration, and then 200 ml of acetonitrile was added and the mixture was heated to reflux under a nitrogen atmosphere for 1 hour. After cooling to room temperature and stirring at room temperature for 1 hour, the solid was collected by filtration and washed with 100 ml of acetonitrile to obtain 2.1 g (yield 79%) of compound A-104. In addition, proton nuclear magnetic resonance ( 1 H-NMR, solvent: deuterated dimethyl sulfoxide (dDMSO) gave chemical shifts δ 11.6 (s, 2H), 7.29 (m, 10H), and 4.80 (s, 4H).

[0294] (Synthesis Example 3) Synthesis of Compound A-1 Compound A-1 was synthesized according to the following synthesis scheme. 1.5 g of compound A-104, 0.76 g of triethylamine, 1.0 g of 2-ethylhexanoyl chloride, and 30 ml of dimethylacetamide were mixed and stirred at 20°C for 1 hour. After the reaction was completed, 30 ml of water was added and stirred for 30 minutes. The precipitated solid was collected by filtration, washed with 30 ml of methanol, and purified by silica gel column chromatography to obtain 1.6 g of compound A-1 (yield 75%). In addition, proton nuclear magnetic resonance ( 1 H-NMR, solvent: deuterated chloroform (CDCl 3 )) had chemical shifts δ 7.27 (m, 6H), 7.10 (m, 4H), 4.75 (s, 4H), 2.69 (m, 2H), 1.8-1.6 (m, 8H), 1.5-1.3 (m, 8H), 1.10 (m, 6H), 0.94 (m, 6H).

[0295] <Regarding Ultraviolet Absorbers> In the test examples shown below, the exemplary compounds (1) to (26) and comparative compounds (1) to (2) used as ultraviolet absorbers are compounds having the structures shown below.

[0296] <Regarding Anti-Fade Agents> In the test examples shown below, compounds T-1 to T-12 used as anti-fade agents are compounds having the structures shown below.

[0297] Test Example 1 The following components were mixed to prepare each composition: UV absorber (compounds shown in the table below (exemplary compounds (1) to (21), comparative compounds (1) to (2))) 1.1 parts by mass Resin (Dianal BR-80, manufactured by Mitsubishi Chemical Corporation, containing 60% by mass or more of methyl methacrylate as monomer units, weight-average molecular weight 95,000) 12.6 parts by mass Anti-fading agent (compounds shown in the table below) 1.1 parts by mass Solvent (chloroform) 85.2 parts by mass

[0298]

[0299] Each of the obtained compositions was spin-coated onto a glass substrate and then dried at 110° C. for 2 minutes to form a film.

[0300] (Evaluation of long-wavelength ultraviolet ray absorption ability) The absorbance of the obtained films was measured using a spectrophotometer (UV-1800PC, manufactured by Shimadzu Corporation). The maximum absorption wavelength (λmax) was measured from the absorption spectrum of each film, and the long-wavelength ultraviolet ray absorption ability was evaluated according to the following criteria. The value in parentheses in the column for long-wavelength ultraviolet ray absorption ability is the value of λmax, and the value in parentheses in the column for colorability is the absorbance ratio A 440 -Evaluation criteria for long wavelength ultraviolet absorption ability- A: λmax is 390 nm or more B: λmax is 380 nm or more but less than 390 nm C: λmax is less than 380 nm

[0301] (Evaluation of Coloring Properties) The absorbance of the obtained film was measured using a spectrophotometer (UV-1800PC, manufactured by Shimadzu Corporation), and the ratio of the absorbance at a wavelength of 440 nm to the absorbance at a wavelength of 400 nm was calculated (absorbance ratio A 440 The absorbance ratio A was calculated and the coloring property (coloring property 1) was evaluated according to the following criteria. 440 The smaller the value, the less coloring there is. Next, a light resistance test was performed on the obtained film under the following condition 1. After the light resistance test, the film was measured for absorbance using a spectrophotometer (UV-1800PC, manufactured by Shimadzu Corporation). The absorbance at a wavelength of 400 nm was taken as 1, and the ratio of the absorbance at a wavelength of 440 nm (absorbance ratio A 440 The values ​​in parentheses in the coloring column are the absorbance ratio A 440 The absorbance ratio A 440 A: Absorbance ratio A A: The smaller the value, the less coloring occurs. 440 is 0.01 or less B: absorbance ratio A 440 is greater than 0.01 C: absorbance ratio A 440 is greater than 0.02

[0302] -Condition 1- Apparatus: Low-temperature cycle xenon weather meter (XL75, manufactured by Suga Test Instruments Co., Ltd.) Illuminance: 90 klx (40 w / m 2 ) Time: 4 weeks Environment: 23°C, relative humidity 50%

[0303] (Evaluation of Lightfastness) A lightfastness test was performed on each film under the above condition 1, and the lightfastness was evaluated by determining the absorbance retention rate at the maximum absorption wavelength (λmax). Specifically, the absorbance of the film at λmax was measured using a spectrophotometer (UV-1800PC, manufactured by Shimadzu Corporation), and then the film was subjected to a lightfastness test under condition 1, and the absorbance of the film after the lightfastness test at λmax was measured. Next, the absorbance retention rate (%) was calculated using the absorbance values ​​at λmax of the film before and after the lightfastness test according to the following formula, and lightfastness was evaluated according to the following criteria. A higher absorbance retention rate means better lightfastness. The evaluation results are shown in the table below. The number in parentheses in the lightfastness column is the value of the absorbance retention rate. Absorbency retention rate (%) = (absorbency at λmax of film after lightfastness test / absorbency at λmax of film before lightfastness test) x 100 - Evaluation criteria - AA: Absorbency retention rate is 90% or more A: Absorbency retention rate is 85% or more B: Absorbency retention rate is 80% or more but less than 85% C: Absorbency retention rate is less than 80%

[0304]

[0305] As shown in the above table, Examples 101 to 166 were excellent in long wavelength ultraviolet absorption ability. 440 Furthermore, the absorbance retention rate after the light fastness test was high, and the evaluation of light fastness was also excellent.

[0306] Test Example 2 The following components were mixed to prepare a composition. UV absorber (compound listed in the table below) 0.6 parts by mass Polymerizable compound (KAYARAD DPHA (manufactured by Nippon Kayaku Co., Ltd., compound having two or more ethylenically unsaturated bond-containing groups) 10.9 parts by mass Resin (DIANAL BR-80 (manufactured by Mitsubishi Chemical Corporation)) 13.4 parts by mass Photopolymerization initiator (compound listed in the table below) 0.6 parts by mass Anti-fading agent (compound listed in the table below) 0.8 parts by mass Solvent (propylene glycol monomethyl ether acetate) 73.7 parts by mass

[0307]

[0308] (Photopolymerization initiators) V-1: Irgacure OXE01 (manufactured by BASF, oxime compound, photoradical polymerization initiator) V-2: Omnirad 2959 (manufactured by IGM Resins B.V., hydroxyacetophenone compound, photoradical polymerization initiator) V-3: Omnirad TPO (manufactured by IGM Resins B.V., acylphosphine compound, photoradical polymerization initiator)

[0309] Each composition was spin-coated onto a 50 mm x 50 mm glass substrate (1737, Corning Incorporated) so that the film thickness after deposition would be 1.5 μm, and then dried at 120°C for 5 minutes to form a composition layer. Thereafter, the composition layer was exposed to an i-line stepper exposure system (UX-1000SM-EH04, Ushio Inc.) at 1000 mJ / cm 2 In Examples 201 to 243, the change in transmittance at the maximum absorption wavelength (λmax) of the composition layer before and after exposure was 5% or less.

[0310] (Evaluation of Coloring Property) The coloring property of the obtained film was evaluated by the same method and criteria as in the evaluation of coloring property in Test Example 1.

[0311] (Evaluation of Light Fastness) A light fastness test was carried out on the obtained film under the following condition 2, and the retention rate of absorbance at the maximum absorption wavelength (λmax) of the film before and after the light fastness test was determined in the same manner as in the evaluation of light fastness in Test Example 1, and the light fastness was evaluated according to the following evaluation criteria.

[0312] -Condition 2- Apparatus: Low-temperature cycle xenon weather meter (XL75, manufactured by Suga Test Instruments Co., Ltd.) Illuminance: 90 klx (40 w / m 2 ) Time: 7 days Environment: 23°C, relative humidity 50%

[0313] - Light resistance evaluation criteria - AA: Absorbency maintenance rate is 80% or more A: Absorbency maintenance rate is 70% or more B: Absorbency maintenance rate is 60% or more but less than 70% C: Absorbency maintenance rate is less than 60%

[0314]

[0315] As shown in the above table, Examples 201 to 253 exhibited an absorbance ratio A 440 Furthermore, the absorbance retention rate after the light fastness test was high, and the evaluation of light fastness was also excellent.

[0316] <Synthesis of Polymer> (Synthesis Example 101) Synthesis of Polymer P-1 To a 200 mL three-neck flask were added 100 mg of compound A-142 (maximum absorption wavelength (in ethyl acetate solution): 394 nm), 9.9 g of methyl methacrylate, and 40.0 g of propylene glycol monomethyl ether acetate, followed by stirring at 80°C for 30 minutes under a nitrogen stream. To this solution was added 200 mg of 2,2'-azobis(isobutyrate)dimethyl (V-601, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. (hereinafter referred to as V-601)), followed by stirring at 80°C for 6 hours and then cooling to room temperature. The resulting reaction mixture was slowly added to a mixture of 140 mL of hexane and 60 mL of isopropyl alcohol and allowed to stand overnight. The precipitate was collected by filtration and washed with a mixture of hexane and isopropyl alcohol. To the resulting powder, 140 mL of hexane and 60 mL of isopropyl alcohol were added, followed by stirring at room temperature for 1 hour and then allowing to stand at room temperature overnight. The precipitate was collected by filtration, washed with a mixture of hexane and isopropyl alcohol, and dried at 50°C to obtain 7.0 g of the target polymer P-1. The number average molecular weight of the obtained polymer P-1 was 27,500 (polystyrene equivalent). 100 mg of the obtained polymer P-1 was dissolved in 100 mL of chloroform, and the absorption spectrum was measured. The maximum absorption wavelength of polymer P-1 was 399 nm (absorbance 1.61). Polymer P-1 was able to sufficiently shield light with a wavelength in the vicinity of 400 nm. Furthermore, polymer P-1 was little colored.

[0317] Synthesis Example 102: Synthesis of Polymer P-2 To a 200 mL three-neck flask were added 100 mg of compound A-142 (maximum absorption wavelength (in ethyl acetate solution): 394 nm), 100 mg of 2-[2-hydroxy-5-(2-methacryloyloxyethyl)phenyl]2H-benzo[d][1,2,3]triazole (maximum absorption wavelength (in ethyl acetate solution): 338 nm) as an ultraviolet absorber, 9.8 g of methyl methacrylate, and 40.0 g of propylene glycol monomethyl ether acetate. The mixture was stirred at 80°C for 6 hours under a nitrogen stream and then cooled to room temperature. The resulting reaction mixture was slowly added to a mixture of 140 mL of hexane and 60 mL of isopropyl alcohol and allowed to stand overnight. The precipitate that separated out was collected by filtration and washed with a mixture of hexane and isopropyl alcohol. To the resulting powder, 140 mL of hexane and 60 mL of isopropyl alcohol were added, and the mixture was stirred at room temperature for 1 hour and then allowed to stand at room temperature overnight. The precipitate was collected by filtration, washed with a mixture of hexane and isopropyl alcohol, and dried at 50°C to obtain 5.0 g of the target polymer P-2. The number average molecular weight of the obtained polymer P-2 was 33,400 (polystyrene equivalent). 150 mg of the obtained polymer P-2 was dissolved in 100 mL of chloroform, and the absorption spectrum was measured. The maximum absorption wavelengths of polymer P-2 were 399 nm (absorbance 1.45) and 343 nm (absorbance 0.83). Polymer P-2 was able to sufficiently shield light with a wavelength in the vicinity of 400 nm. Furthermore, it also had excellent shielding properties for light with a wavelength shorter than 350 nm. Furthermore, polymer P-2 was little colored.

[0318] Synthesis Example 103: Synthesis of Polymer P-3 To a 200 mL three-neck flask were added 100 mg of compound A-142 (maximum absorption wavelength (in ethyl acetate solution): 394 nm), 9.9 g of butyl methacrylate, and 40.0 g of propylene glycol monomethyl ether acetate, and the mixture was stirred at 80°C for 30 minutes under a nitrogen stream. To this solution was added 20 mg of 2,2'-azobis(isobutyrate)dimethyl (V-601, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. (hereinafter referred to as V-601)), and the mixture was stirred at 80°C for 6 hours and then cooled to room temperature. The resulting reaction mixture was slowly added to a mixture of 200 mL of methanol and allowed to stand overnight. The precipitate was collected by filtration and washed with a mixture of chloroform and methanol. 20 mL of chloroform and 200 mL of methanol were added to the obtained powder, and the mixture was stirred at room temperature for 1 hour and then allowed to stand at room temperature overnight. The precipitate was collected by filtration, washed with a mixture of chloroform and methanol, and dried at 50°C to obtain 5.2 g of the target polymer P-3. The number average molecular weight of the obtained polymer P-3 was 96,000 (polystyrene equivalent). 100 mg of the obtained polymer P-3 was dissolved in 100 mL of chloroform, and the absorption spectrum was measured. The maximum absorption wavelength of polymer P-3 was 399 nm (absorbance 1.56). Polymer P-3 was able to sufficiently shield light with a wavelength in the vicinity of 400 nm. Furthermore, polymer P-3 was little colored.

[0319] Synthesis Example 104: Synthesis of Polymer P-4 To a 200 mL three-neck flask were added 100 mg of compound A-232 (maximum absorption wavelength (in ethyl acetate solution): 391 nm), 9.9 g of methyl methacrylate, and 40.0 g of propylene glycol monomethyl ether acetate, and the mixture was stirred at 80°C for 30 minutes under a nitrogen stream. To this solution was added 200 mg of 2,2'-azobis(isobutyrate)dimethyl (V-601, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. (hereinafter referred to as V-601)), and the mixture was stirred at 80°C for 6 hours and then cooled to room temperature. The resulting reaction mixture was slowly added to a mixture of 140 mL of hexane and 60 mL of isopropyl alcohol and allowed to stand overnight. The precipitate was collected by filtration and washed with a mixture of hexane and isopropyl alcohol. To the resulting powder, 140 mL of hexane and 60 mL of isopropyl alcohol were added, and the mixture was stirred at room temperature for 1 hour and then allowed to stand at room temperature overnight. The precipitate was collected by filtration, washed with a mixture of hexane and isopropyl alcohol, and dried at 50°C to obtain 7.4 g of the target polymer P-4. The number average molecular weight of the obtained polymer P-4 was 29,500 (polystyrene equivalent). 100 mg of the obtained polymer P-4 was dissolved in 100 mL of chloroform, and the absorption spectrum was measured. The maximum absorption wavelength of polymer P-4 was 397 nm (absorbance 1.57). Polymer P-4 was able to sufficiently shield light with a wavelength in the vicinity of 400 nm. Furthermore, polymer P-4 was little colored.

[0320] Synthesis Example 105: Synthesis of Polymer P-5 To a 200 mL three-neck flask were added 100 mg of compound A-352 (maximum absorption wavelength (in ethyl acetate solution): 392 nm), 9.9 g of methyl methacrylate, and 40.0 g of propylene glycol monomethyl ether acetate, and the mixture was stirred at 80°C for 30 minutes under a nitrogen stream. To this solution was added 200 mg of 2,2'-azobis(isobutyrate)dimethyl (V-601, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. (hereinafter referred to as V-601)), and the mixture was stirred at 80°C for 6 hours and then cooled to room temperature. The resulting reaction mixture was slowly added to a mixture of 140 mL of hexane and 60 mL of isopropyl alcohol and allowed to stand overnight. The precipitate was collected by filtration and washed with a mixture of hexane and isopropyl alcohol. To the resulting powder, 140 mL of hexane and 60 mL of isopropyl alcohol were added, and the mixture was stirred at room temperature for 1 hour and then allowed to stand at room temperature overnight. The precipitate was collected by filtration, washed with a mixture of hexane and isopropyl alcohol, and dried at 50°C to obtain 7.8 g of the target polymer P-5. The number average molecular weight of the obtained polymer P-5 was 45,000 (polystyrene equivalent). 100 mg of the obtained polymer P-5 was dissolved in 100 mL of chloroform, and the absorption spectrum was measured. The maximum absorption wavelength of polymer P-5 was 397 nm (absorbance 1.47). Polymer P-5 was able to sufficiently shield light with a wavelength in the vicinity of 400 nm. Furthermore, polymer P-5 was little colored.

[0321] (Comparative Synthesis Example 101) Synthesis of Polymer P-6 To a 200 mL three-neck flask, 104 mg of 2-[2-hydroxy-5-(2-methacryloyloxyethyl)phenyl]2H-benzo[d][1,2,3]triazole, 9.9 g of methyl methacrylate, and 40.0 g of propylene glycol monomethyl ether acetate were added and stirred at 80°C for 30 minutes under a nitrogen stream. 135 mg of V-601 was added to this solution and stirred at 80°C for 4 hours. An additional 37 mg of V-601 was added, and the mixture was stirred at 90°C for 2 hours and then cooled to room temperature. The resulting reaction mixture was slowly added to a mixture of 140 mL of hexane and 60 mL of isopropyl alcohol. The precipitate was collected by filtration and washed with a mixture of hexane and isopropyl alcohol. To the obtained powder, 140 mL of hexane and 60 mL of isopropyl alcohol were added, and the mixture was stirred at room temperature for 3 hours. The precipitate was collected by filtration, washed with a mixture of hexane and isopropyl alcohol, and dried at 50°C to obtain 8.1 g of the target polymer P-6. The number average molecular weight of the obtained polymer P-6 was 14,100 (polystyrene equivalent). 150 mg of polymer P-6 was dissolved in 100 mL of chloroform, and the absorption spectrum was measured. The maximum absorption wavelength of polymer P-6 was 339 nm (absorbance 0.91). Polymer P-6 had low light shielding ability in the wavelength range of 380 to 400 nm.

[0322] Test Example 3 (Examples 301 to 310, Comparative Examples 301 and 302) A composition (resin composition (resin solution)) was prepared by dissolving 500 mg of a polymer shown in the table below, 5.1 mg of a discoloration inhibitor shown in the table below, 7.6 g of chloroform, and 1.1 g of polymethyl methacrylate resin (Dianal BR-80 (containing 60% by mass or more of methyl methacrylate as a monomer unit, weight average molecular weight: 95,000, acid value: 0 mgKOH / g, manufactured by Mitsubishi Chemical Corporation)). The obtained composition was spin-coated onto a glass substrate, and the coated film was dried at 60°C for 2 minutes to form a film with a thickness of approximately 10 μm. The films obtained using the compositions of Examples 301 to 308 were almost free of coloration and had excellent light-shielding properties with wavelengths around 400 nm, whereas the films obtained using the compositions of Comparative Examples 301 and 302 had poor light-shielding properties with wavelengths of 380 to 400 nm.

[0323] (Evaluation of Coloring Property) The coloring property of the obtained film was evaluated by the same method and criteria as in the evaluation of coloring property in Test Example 1.

[0324] (Evaluation of Lightfastness) The lightfastness of the obtained film was evaluated by the same method and evaluation criteria as in Test Example 1, except that the lightfastness test was conducted under the following Condition 3. -Condition 3- Apparatus: Low-temperature cycle xenon weather meter (XL75, manufactured by Suga Test Instruments Co., Ltd.) Illuminance: 90 klx (40 W / m 2 ) Time: 4 weeks Environment: 23°C, relative humidity 5%

[0325]

[0326] As shown in the table above, Examples 301 to 310 exhibited an absorbance ratio A 440 Furthermore, the absorbance retention rate after the light fastness test was high, and the evaluation of light fastness was also excellent.

[0327] Test Example 4 120 mg of an ultraviolet absorber shown in the table below, an anti-fading agent shown in the table below, 120 mg of Irgacure OXE01 (manufactured by BASF, oxime compound, photoradical polymerization initiator), 15.9 g of propylene glycol methyl ether acetate, 2.84 g of a (meth)acrylic resin (Dianal BR-80, manufactured by Mitsubishi Chemical Corporation, containing 60% by mass or more of methyl methacrylate as monomer units, Mw 95000), and 2.32 g of KAYARAD DPHA (manufactured by Nippon Kayaku Co., Ltd., compound having two or more ethylenically unsaturated bond-containing groups) were mixed and dissolved to prepare a composition.

[0328]

[0329] Each composition was spin-coated onto a 50 mm x 50 mm glass substrate (1737, Corning Incorporated) so that the film thickness after deposition would be 1.5 μm, and then dried at 120°C for 5 minutes to form a composition layer. Thereafter, the composition layer was exposed to an i-line stepper exposure system (UX-1000SM-EH04, Ushio Inc.) at 1000 mJ / cm 2In Examples 401 to 421, the change in transmittance at the maximum absorption wavelength (λmax) of the composition layer before and after exposure was 5% or less.

[0330] (Evaluation of Coloring Property) The coloring property of the obtained film was evaluated by the same method and criteria as in the evaluation of coloring property in Test Example 1.

[0331] (Evaluation of Light Resistance) The light resistance of the obtained film was evaluated by the same method and criteria as in the evaluation of light resistance in Test Example 2.

[0332]

[0333] As shown in the above table, Examples 401 to 436 exhibited an absorbance ratio A 440 Furthermore, the absorbance retention rate after the light fastness test was high, and the evaluation of light fastness was also excellent.

Claims

1. A composition comprising an ultraviolet absorber, a curable compound, and a discoloration inhibitor, the ultraviolet absorber comprising at least one selected from the group consisting of a compound represented by formula (1) and a polymer comprising a structure derived from the compound represented by formula (1), and the discoloration inhibitor comprising at least one selected from the group consisting of an amine compound, a phenol compound, a hydroquinone compound, a catechol compound, an ascorbic acid compound, a carotenoid compound, a metal complex compound, and a benzolactone compound; In formula (1), Q 1 represents a group represented by formula (Q-1); Q 2 =O, =S, =NR q1 Or = CR q2 R q3 represents R q1 ~R q3 each independently represents a hydrogen atom or a substituent; R q2 and R q3 may be bonded to each other to form a ring; provided that R q2 and R q3 When they are bonded to form a ring, ═CR q2 R q3 Q 1 is not identical in structure to; 1 and R 2 each independently represents a hydrogen atom or a substituent; X 1 ~X 4 Each independently represents -S-, -NR X1 - or -SO 2 - represents R X1 represents a hydrogen atom or an alkyl group; In formula (Q-1), * represents a bond; 101 and R 102 each independently represents a hydrogen atom, an alkyl group, an aralkyl group, an aryl group, a heterocyclic group, or a group containing a polymerizable group having an ethylenically unsaturated bond; 101 Or R 102 When either one of R is a hydrogen atom, the other represents an alkyl group, an aralkyl group, an aryl group, a heterocyclic group, or a group containing a polymerizable group having an ethylenically unsaturated bond, 101 Or R 102 When either one of R is a methyl group, the other represents a hydrogen atom, an alkyl group having two or more carbon atoms, an aralkyl group, an aryl group, a heterocyclic group, or a group containing a polymerizable group having an ethylenically unsaturated bond, 101 Or R 102 When one of the above is a phenyl group, the other represents a hydrogen atom, an alkyl group, an aralkyl group, an aryl group having a substituent, a heterocyclic group, or a group containing a polymerizable group having an ethylenically unsaturated bond.

2. The composition according to claim 1, wherein the compound represented by formula (1) is a compound represented by formula (3); In formula (3), Q 3 represents a group represented by formula (Q-1); Q 4 =O, =S, =NR q11 Or = CR q12 R q13 represents R q11 ~R q13 each independently represents a hydrogen atom or a substituent; R q12 and R q13 may be bonded to each other to form a ring; provided that R q12 and R q13 When they are bonded to form a ring, ═CR q12 R q13 Q 3 is not identical in structure to; 11 and R 12 each independently represents -OH, -O-Y 11 , -OC(=O)-Y 11 , -OC(=O)O-Y 11 , -OC(=O)NR y11 -Y 11 , -OSO 2 -Y 11 or a group containing a polymerizable group having an ethylenically unsaturated bond, R y11 represents a hydrogen atom, an alkyl group, an aralkyl group, or an aryl group; Y 11 represents an alkyl group, an aralkyl group, or an aryl group.

3. The composition according to claim 1 or 2, wherein the anti-fading agent comprises at least one selected from the group consisting of a compound represented by formula (Ao1-1) and a compound represented by formula (Ao2-1). In formula (Ao1-1), R a1 ~R a4 each independently represents a hydrogen atom, an alkyl group, or an alkenyl group; a1 represents a hydrogen atom, an alkyl group, an alkenyl group, an alkoxy group, an alkenyloxy group, an alkoxycarbonyl group, an alkenyloxycarbonyl group, an aryloxycarbonyl group, an acyl group, an acyloxy group, an alkoxycarbonyloxy group, an alkenyloxycarbonyloxy group, an aryloxycarbonyloxy group, an alkylsulfonyl group, an alkenylsulfonyl group, an arylsulfonyl group, an alkylsulfinyl group, an alkenylsulfinyl group, an arylsulfinyl group, a sulfamoyl group, a carbamoyl group, a hydroxy group, or an oxy radical group; X a2 represents an atomic group necessary to form a 5- to 7-membered ring; p1 represents a hydrogen atom, an alkyl group, an alkenyl group, an aryl group, a heterocyclic group, an acyl group, an alkoxycarbonyl group, an alkenyloxycarbonyl group, an aryloxycarbonyl group, an alkylsulfonyl group, an arylsulfonyl group, or -Si(R p101 ) (R p102 ) (R p103 ), R p101 ~R p103 each independently represents an alkyl group, an alkenyl group, an aryl group, an alkoxy group, an alkenyloxy group, or an aryloxy group; R p2 ~R p6 each independently represents a hydrogen atom or a substituent; R p1 ~R p6 Any two adjacent groups among R may be bonded to each other to form a ring; p1 ~R p6 Not all of the atoms are hydrogen atoms.

4. The composition according to claim 1 or 2, wherein the anti-fading agent comprises at least one selected from the group consisting of a compound represented by formula (Ao1-2) and a compound represented by formula (Ao2-2); In formula (Ao1-2), X a11 represents a hydrogen atom, an alkyl group, an alkenyl group, an alkoxy group, an alkenyloxy group, an alkoxycarbonyl group, an alkenyloxycarbonyl group, an aryloxycarbonyl group, an acyl group, an acyloxy group, an alkoxycarbonyloxy group, an alkenyloxycarbonyloxy group, an aryloxycarbonyloxy group, an alkylsulfonyl group, an alkenylsulfonyl group, an arylsulfonyl group, an alkylsulfinyl group, an alkenylsulfinyl group, an arylsulfinyl group, a sulfamoyl group, a carbamoyl group, a hydroxy group, or an oxy radical group; R a11 represents a substituent; In formula (Ao2-2), R p11 ~R p14 each independently represents a hydrogen atom, an alkyl group, or an alkenyl group; Y p11 represents an aryl group, a heteroaryl group, or an ethylenically unsaturated bond-containing group.

5. The composition according to claim 1 or 2, wherein the curable compound comprises at least one selected from a resin and a polymerizable compound.

6. The composition according to claim 1 or 2, wherein the curable compound contains a resin, and the resin is at least one selected from the group consisting of (meth)acrylic resin, polystyrene resin, polyester resin, polyurethane resin, thiourethane resin, polyimide resin, epoxy resin, polycarbonate resin, phthalate resin, cellulose acylate resin and cyclic olefin resin.

7. A cured product obtained by using the composition according to claim 1 or 2.

8. An optical component comprising the cured product according to claim 7.

Citation Information

Patent Citations

  • Ultraviolet absorbing agent composition

    JP2009067984A

  • Liquid crystal composition comprising polymerizable liquid crystal compound and stabilizer

    JP2009242718A

  • Heterocyclic compound, ultraviolet ray absorbent, and composition comprising the ultraviolet ray absorbent

    WO2009022736A1

  • Coloring composition, inkjet recording ink and heterocyclic compound

    WO2009022738A1

  • Photopolymerizable composition, cured article, and optical member

    WO2022239762A1