Laminate and packaging material
The laminate, featuring a polyolefin and (meth)acrylic resin sealing layer and a polyurethane gas barrier layer, addresses the challenge of balancing handling and bending resistance, offering enhanced performance in packaging applications with improved gas barrier and heat sealability.
Patent Information
- Application Number
- PCT/JP2024/010896
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional laminates used for packaging require balancing excellent handling properties and bending resistance, which existing technologies fail to achieve simultaneously, especially in applications requiring gas barrier and heat sealability.
A laminate comprising a paper base material with a sealing layer containing a polyolefin resin and a (meth)acrylic resin, and a gas barrier layer made from a polyurethane resin with a reaction product of an isocyanate group-terminated prepolymer and a chain extender, optionally including a heat seal layer for enhanced performance.
The laminate achieves both excellent handling properties and bending resistance, while providing effective gas barrier and heat sealability, making it suitable for various industrial applications, including food packaging.
Smart Images

Figure JP2024010896_03102024_PF_FP_ABST
Abstract
Description
Laminates and packaging materials
[0001] The present invention relates to a laminate and a packaging material, and more particularly to a laminate including a sealing layer and a gas barrier layer.
[0002] BACKGROUND ART Laminates comprising a paper substrate, a sealing layer, and a gas barrier layer have been known in the art, and such laminates are used, for example, as packaging materials.
[0003] More specifically, the following barrier paper has been proposed as a laminate. The barrier paper comprises a paper base layer, a fixed sealing layer, and a gas barrier layer. More specifically, either a styrene-acrylic copolymer aqueous emulsion or a polyethylene resin aqueous emulsion is applied to the paper base to form the fixed sealing layer. Alternatively, a urethane-based hybrid gas barrier resin composition is applied to the fixed sealing layer to form the gas barrier layer (see, for example, Patent Document 1 (Examples A13 to 15 and Comparative Examples A10 to 21)).
[0004] Japanese Patent Application Laid-Open No. 2022-155999
[0005] On the other hand, barrier paper is required to have both excellent handling properties and excellent flex resistance depending on the application.
[0006] The present invention provides a laminate and a packaging material that have both excellent handling properties and excellent flex resistance.
[0007] The present invention [1] includes a laminate comprising a paper base material, a sealing layer disposed on at least one side of the paper base material, and a gas barrier layer disposed on at least one side of the sealing layer, wherein the sealing layer contains a polyolefin resin and a (meth)acrylic resin.
[0008] The present invention [2] includes the laminate according to the above [1], in which the content of the polyolefin resin is 6% by mass or more and 94% by mass or less, and the content of the (meth)acrylic resin is 6% by mass or more and 94% by mass or less, relative to the total amount of the polyolefin resin and the (meth)acrylic resin.
[0009] The present invention [3] includes the laminate according to the above [1] or [2], wherein the glass transition temperature of the (meth)acrylic resin is −60° C. or higher and 10° C. or lower.
[0010] The present invention [4] includes the laminate according to any one of the above [1] to [3], wherein the gas barrier layer contains a gas barrier resin.
[0011] The present invention [5] includes the laminate according to the above [4], wherein the gas barrier resin contains a gas barrier polyurethane resin.
[0012] The present invention [6] includes the laminate according to the above [5], wherein the gas barrier polyurethane resin contains a reaction product of an isocyanate group-terminated prepolymer and a chain extender, the isocyanate group-terminated prepolymer contains a reaction product of a polyisocyanate component and an active hydrogen group-containing component, the polyisocyanate component contains xylylene diisocyanate and / or hydrogenated xylylene diisocyanate, and the active hydrogen group-containing component contains a short-chain diol having 2 to 6 carbon atoms and an active hydrogen compound containing an anionic group.
[0013] The present invention [7] includes the laminate according to any one of the above [4] to [6], wherein the gas barrier layer further contains a layered inorganic compound.
[0014] The present invention [8] includes the laminate according to any one of the above [1] to [7], further comprising a heat seal layer disposed on at least one side of the gas barrier layer.
[0015] The present invention [9] includes a packaging material containing the laminate according to any one of the above [1] to [8].
[0016] The laminate of the present invention includes a paper substrate, a sealing layer, and a gas barrier layer. In the laminate, the sealing layer contains a polyolefin resin and a (meth)acrylic resin. Therefore, the sealing layer has excellent blocking resistance. That is, the laminate has excellent handleability. Furthermore, since the sealing layer contains a polyolefin resin and a (meth)acrylic resin, it has excellent flex resistance. As a result, the laminate has both excellent handleability and excellent flex resistance.
[0017] The packaging material of the present invention contains the above laminate, and therefore has both excellent handling properties and excellent flex resistance.
[0018] FIG. 1 is a schematic diagram showing one embodiment of the laminate of the present invention.
[0019] 1. Laminate In FIG. 1, the laminate 1 includes a paper base material 2, a filling layer 3 disposed on at least one side in the thickness direction of the paper base material 2 (upper side in the drawing), and a gas barrier layer 4 disposed on at least one side in the thickness direction of the filling layer 3 (upper side in the drawing).
[0020] Furthermore, the laminate 1 can further include, as an optional layer, a heat seal layer 5 disposed on at least one side in the thickness direction of the gas barrier layer 4 (upper side in the drawing). In Fig. 1, the laminate 1 includes a heat seal layer 5. That is, in Fig. 1, the laminate 1 includes a paper base material 2, a sealing layer 3, a gas barrier layer 4, and a heat seal layer 5, in that order from the other side in the thickness direction (lower side in the drawing) to one side (upper side in the drawing).
[0021] (1) Paper Base Material The paper base material 2 is a base material formed from paper. Examples of the paper base material 2 include paper made from pulp. Examples of pulp include natural pulp and synthetic pulp. More specific examples of the paper base material 2 include glassine paper, coated paper, one-side gloss kraft paper, roll paper, and cup base paper. The paper base material 2 may be a single-layer paper or may be a multi-layer paper. The paper base material 2 is appropriately selected depending on the application of the laminate 1.
[0022] The shape of the paper substrate 2 is not particularly limited and may be appropriately set. Examples of the shape of the paper substrate 2 include a sheet shape, a bottle shape, and a cup shape. A preferred shape of the paper substrate 2 is a sheet shape.
[0023] The paper substrate 2 may be subjected to a surface treatment as required, such as a corona discharge treatment, a surface coating treatment, or a vapor deposition treatment.
[0024] The thickness of the paper base material 2 is, for example, 3 μm or more, or preferably 5 μm or more, and for example, 500 μm or less, or preferably 200 μm or less.
[0025] The basis weight of the paper base material 2 is, for example, 20 g / m 2 More than 30 g / m 2 The basis weight of the paper base material 2 is, for example, 400 g / m 2 Preferably, 300 g / m or less 2 The following is the result.
[0026] (2) Filler layer The filler layer 3 is laminated on the paper base material 2 to suppress impregnation of the gas barrier coating material (described later) into the paper base material 2. The filler layer 3 is also laminated on the paper base material 2 to absorb unevenness on the surface of the paper base material 2 and smooth the surface. More specifically, the filler layer 3 is disposed on at least one surface of the paper base material 2. The filler layer 3 may be disposed on both surfaces of the paper base material 2. The filler layer 3 is preferably disposed on only one surface of the paper base material 2.
[0027] The filling layer 3 contains a filling resin. More specifically, the filling layer 3 is formed, for example, by applying a coating material containing a filling resin (hereinafter referred to as a filling coating material) to the surface of the paper base material 2 and drying it.
[0028] More specifically, examples of the sealing coating material include a solution obtained by dissolving a sealing resin in a solvent (described later), and a dispersion obtained by dispersing a sealing resin in a solvent (described later).
[0029] Examples of the sealing resin include a polyolefin resin and a (meth)acrylic resin. More specifically, the sealing resin (sealing layer 3) contains a polyolefin resin and a (meth)acrylic resin as essential components. That is, a polyolefin resin and a (meth)acrylic resin are used in combination as the sealing resin.
[0030] [Polyolefin Resin (PO)] Polyolefin resin is a resin containing structural units derived from olefins, and is obtained by polymerization of monomer components (hereinafter referred to as olefin raw material monomer components) as a raw material composition.
[0031] The olefin raw material monomer component contains an olefin. Examples of the olefin include α-olefins. Examples of the α-olefin include α-olefins having 1 to 20 carbon atoms. Examples of the α-olefins having 1 to 20 carbon atoms include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene. These can be used alone or in combination of two or more. As the α-olefin, preferably, an olefin having 2 to 3 carbon atoms is used, more preferably, ethylene and / or propylene is used, and even more preferably, ethylene is used.
[0032] The olefin feedstock monomer component may contain only an olefin. Alternatively, the olefin feedstock monomer component may contain an olefin and a copolymerizable monomer. Preferably, the olefin feedstock monomer component contains an olefin and a copolymerizable monomer.
[0033] In the olefin raw material monomer component, the copolymerizable monomer is a monomer copolymerizable with an olefin. Examples of the copolymerizable monomer include unsaturated carboxylic acids, unsaturated carboxylic acid esters, hydroxyl group-containing vinyl monomers, amino group-containing vinyl monomers, glycidyl group-containing vinyl monomers, cyano group-containing vinyl monomers, sulfonic acid group-containing vinyl monomers, acetoacetoxy group-containing vinyl monomers, phosphoric acid group-containing vinyl monomers, amide group-containing vinyl monomers, aromatic vinyl monomers, N-substituted unsaturated carboxylic acid amides, heterocyclic vinyl compounds, vinylidene halide compounds, dienes, and vinyl esters. These can be used alone or in combination of two or more.
[0034] As the copolymerizable monomer, preferably, an unsaturated carboxylic acid is used. When the olefin raw material monomer component contains an unsaturated carboxylic acid, excellent water dispersibility can be obtained.
[0035] Examples of unsaturated carboxylic acids include unsaturated monocarboxylic acids and unsaturated dicarboxylic acids. Examples of unsaturated monocarboxylic acids include (meth)acrylic acid, crotonic acid, and isocrotonic acid. Examples of unsaturated dicarboxylic acids include maleic acid, fumaric acid, tetrahydrophthalic acid, itaconic acid, citraconic acid, and norbornene dicarboxylic acid, and their acid anhydrides. The unsaturated carboxylic acids can be used alone or in combination of two or more. Preferable examples of unsaturated carboxylic acids include unsaturated monocarboxylic acids and acid anhydrides of unsaturated dicarboxylic acids, and more preferably (meth)acrylic acid.
[0036] The term "(meth)acrylic" refers to acrylic and / or methacrylic. The same applies to "(meth)acrylate." As the (meth)acrylic acid, methacrylic acid is preferred.
[0037] When the olefin raw material monomer component contains an olefin and an unsaturated carboxylic acid, an unsaturated carboxylic acid-modified polyolefin resin is obtained as the polyolefin resin. More specifically, an example of the unsaturated carboxylic acid-modified polyolefin resin is ethylene-methacrylic acid copolymer (EMAA).
[0038] In the olefin raw material monomer component, the content ratio of the olefin to the copolymerizable monomer is appropriately set depending on the type of the copolymerizable monomer. For example, the ratio of the olefin to the unsaturated carboxylic acid as the copolymerizable monomer is appropriately adjusted in order to achieve a balance between the handleability (blocking resistance) and flex resistance of the sealing layer 3 and the hydrophilicity of the polyolefin resin.
[0039] More specifically, the olefin content is, for example, 50% by mass or more, preferably 60% by mass or more, and more preferably 70% by mass or more, relative to the total amount of the olefin raw material monomer components, and, for example, 99% by mass or less, preferably 97% by mass or less, more preferably 95% by mass or less, even more preferably 93% by mass or less, and particularly preferably 90% by mass or less, relative to the total amount of the olefin raw material monomer components.
[0040] The content of the olefin in the olefin raw material monomer component is substantially synonymous with the content of the olefin-derived structural units in the unsaturated carboxylic acid-modified polyolefin resin.
[0041] That is, the content of the olefin-derived structural units is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, relative to the total amount of the unsaturated carboxylic acid-modified polyolefin resin. Also, the content of the olefin-derived structural units is, for example, 99% by mass or less, preferably 97% by mass or less, more preferably 95% by mass or less, even more preferably 93% by mass or less, and particularly preferably 90% by mass or less, relative to the total amount of the unsaturated carboxylic acid-modified polyolefin resin.
[0042] In the polyolefin resin, the content of the olefin-derived structural units is, as described above, 50% by mass or more, preferably 60% by mass or more, based on the total amount of the polyolefin resin. The polyolefin resin is distinguished from other resins containing olefin-derived structural units by the content of the olefin-derived structural units.
[0043] More specifically, in a resin other than a polyolefin resin containing a structural unit derived from an olefin (for example, a (meth)acrylic resin described later), the content of the structural unit derived from an olefin is less than 50% by mass, preferably 40% by mass or less.
[0044] From the viewpoint of hydrophilicity, the content of the unsaturated carboxylic acid is, for example, 1% by mass or more, preferably 5% by mass or more, more preferably 8% by mass or more, and even more preferably 10% by mass or more, relative to the total amount of the olefin raw material monomer components. From the viewpoints of handleability (blocking resistance) and flex resistance, the content of the unsaturated carboxylic acid is, for example, less than 50% by mass, preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 25% by mass or less, relative to the total amount of the olefin raw material monomer components.
[0045] The content of the unsaturated carboxylic acid in the olefin raw material monomer component is substantially synonymous with the content of the structural unit derived from the unsaturated carboxylic acid in the unsaturated carboxylic acid-modified polyolefin resin.
[0046] That is, the content of the structural units derived from the unsaturated carboxylic acid is, for example, 1% by mass or more, preferably 5% by mass or more, more preferably 8% by mass or more, and even more preferably 10% by mass or more, relative to the total amount of the unsaturated carboxylic acid-modified polyolefin resin. Also, the content of the structural units derived from the unsaturated carboxylic acid is, for example, less than 50% by mass, preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 25% by mass or less, relative to the total amount of the unsaturated carboxylic acid-modified polyolefin resin.
[0047] The method for producing the polyolefin resin is not particularly limited, and a known method can be used. For example, the above-mentioned olefin raw material monomer components are contacted with a known polymerization initiator (such as a peroxide) under high temperature and high pressure conditions. This results in a polyolefin resin as a polymerization product of the olefin raw material monomer components.
[0048] [(Meth)acrylic Resin (Ac)] The (meth)acrylic resin is a resin containing a structural unit derived from a (meth)acrylic acid ester. The (meth)acrylic resin is obtained by polymerization of a monomer component (hereinafter referred to as an acrylic raw material monomer component) as a raw material composition.
[0049] The acrylic raw material monomer component contains a (meth)acrylic acid ester. Examples of the (meth)acrylic acid ester include (meth)acrylic acid esters having an alkyl moiety with 1 to 12 carbon atoms. More specific examples of the (meth)acrylic acid ester include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and lauryl (meth)acrylate. These may be used alone or in combination of two or more. As the (meth)acrylic acid ester, preferably, a (meth)acrylic acid ester having an alkyl moiety with 2 to 10 carbon atoms is used, more preferably, a (meth)acrylic acid ester having an alkyl moiety with 4 to 8 carbon atoms is used, still more preferably, butyl (meth)acrylate and 2-ethylhexyl (meth)acrylate are used, and particularly preferably, 2-ethylhexyl (meth)acrylate (also known as 2-ethylhexyl (meth)acrylate) is used.
[0050] The acrylic raw material monomer component may contain only a (meth)acrylic acid ester. Alternatively, the acrylic raw material monomer component may contain a (meth)acrylic acid ester and a copolymerizable monomer. Preferably, the acrylic raw material monomer component contains a (meth)acrylic acid ester and a copolymerizable monomer.
[0051] In the acrylic raw material monomer component, the copolymerizable monomer is a monomer copolymerizable with a (meth)acrylic acid ester. Examples of the copolymerizable monomer include olefins, unsaturated carboxylic acids, hydroxyl group-containing vinyl monomers, amino group-containing vinyl monomers, glycidyl group-containing vinyl monomers, cyano group-containing vinyl monomers, sulfonic acid group-containing vinyl monomers, acetoacetoxy group-containing vinyl monomers, phosphoric acid group-containing vinyl monomers, amide group-containing vinyl monomers, aromatic vinyl monomers, N-substituted unsaturated carboxylic acid amides, heterocyclic vinyl compounds, vinylidene halide compounds, dienes, and vinyl esters. These can be used alone or in combination of two or more.
[0052] As the copolymerizable monomer, an aromatic vinyl monomer is preferably used. When the acrylic raw material monomer component contains an aromatic vinyl monomer, the blocking resistance of the sealing layer 3 is further improved.
[0053] Examples of aromatic vinyl monomers include styrene, α-methylstyrene, t-butylstyrene, halogenated styrene, vinyltoluene, and vinylxylene. These can be used alone or in combination of two or more. Styrene is a preferred aromatic vinyl monomer.
[0054] When the acrylic raw material monomer contains a (meth)acrylic acid ester and an aromatic vinyl monomer, an aromatic ring-containing (meth)acrylic resin is obtained as the (meth)acrylic resin. More specifically, the aromatic ring-containing (meth)acrylic resin may be, for example, a styrene-(meth)acrylic acid ester copolymer.
[0055] In the acrylic raw material monomer component, the content ratio of the (meth)acrylic acid ester and the copolymerizable monomer is appropriately set depending on the type of the copolymerizable monomer. For example, the ratio of the (meth)acrylic acid ester and the aromatic vinyl monomer as the copolymerizable monomer is appropriately adjusted in order to balance the handleability (blocking resistance) and flex resistance of the sealing layer 3 with the glass transition temperature (described later) of the (meth)acrylic resin.
[0056] More specifically, the content of the (meth)acrylic acid ester relative to the total amount of the acrylic raw material monomer components is, for example, 10% by mass or more, preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, even more preferably 50% by mass or more, and particularly preferably 60% by mass or more. The content of the (meth)acrylic acid ester relative to the total amount of the acrylic raw material monomer components is, for example, 99% by mass or less, preferably 90% by mass or less, more preferably 80% by mass or less, even more preferably 85% by mass or less, and particularly preferably 70% by mass or less.
[0057] The content of the (meth)acrylic acid ester in the acrylic raw material monomer component is substantially synonymous with the content of the structural unit derived from the (meth)acrylic acid ester in the (meth)acrylic resin.
[0058] That is, the content of the structural units derived from the (meth)acrylic acid ester, relative to the total amount of the (meth)acrylic resin, is, for example, 10% by mass or more, preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, even more preferably 50% by mass or more, and particularly preferably 60% by mass or more. Also, the content of the structural units derived from the (meth)acrylic acid ester, relative to the total amount of the (meth)acrylic resin, is, for example, 99% by mass or less, preferably 90% by mass or less, more preferably 80% by mass or less, even more preferably 85% by mass or less, and particularly preferably 70% by mass or less.
[0059] From the viewpoints of handleability (blocking resistance) and glass transition temperature, the content of the aromatic vinyl monomer is, for example, 1% by mass or more, preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 25% by mass or more, and particularly preferably 30% by mass or more, relative to the total amount of the acrylic raw material monomer components. From the viewpoints of flex resistance and glass transition temperature, the content of the aromatic vinyl monomer is, for example, 90% by mass or less, preferably 80% by mass or less, more preferably 70% by mass or less, even more preferably 60% by mass or less, even more preferably 50% by mass or less, and particularly preferably 40% by mass or less, relative to the total amount of the acrylic raw material monomer components.
[0060] The content of the aromatic vinyl monomer in the acrylic raw material monomer component is substantially synonymous with the content of the structural unit derived from the aromatic vinyl monomer in the (meth)acrylic resin.
[0061] That is, the content of the structural units derived from aromatic vinyl monomers relative to the total amount of the (meth)acrylic resin is, for example, 1% by mass or more, preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 25% by mass or more, and particularly preferably 30% by mass or more. Also, the content of the structural units derived from aromatic vinyl monomers relative to the total amount of the (meth)acrylic resin is, for example, 90% by mass or less, preferably 80% by mass or less, more preferably 70% by mass or less, even more preferably 60% by mass or less, even more preferably 50% by mass or less, and particularly preferably 40% by mass or less.
[0062] When the acrylic raw material monomer component contains an olefin as a copolymerizable monomer, the content of structural units derived from the olefin in the (meth)acrylic resin is less than 50% by mass, preferably 40% by mass or less, based on the total amount of the (meth)acrylic resin. The (meth)acrylic resin is distinguished from the above-mentioned polyolefin resin by the content of structural units derived from the olefin.
[0063] In the acrylic raw material monomer component, the types and proportions of the (meth)acrylic acid ester and copolymerizable monomer are set in order to adjust the glass transition temperature of the (meth)acrylic resin.
[0064] The glass transition temperature of the (meth)acrylic resin is, for example, −90° C. or higher, preferably −60° C. or higher, more preferably −50° C. or higher, even more preferably −40° C. or higher, and particularly preferably −30° C. or higher. The glass transition temperature of the (meth)acrylic resin is, for example, 70° C. or lower, preferably 50° C. or lower, more preferably 30° C. or lower, even more preferably 10° C. or lower, even more preferably 0° C. or lower, and particularly preferably −10° C. or lower. When the glass transition temperature of the (meth)acrylic resin is within the above range, particularly excellent blocking resistance can be obtained.
[0065] The glass transition temperature of the (meth)acrylic resin is calculated based on the Fox equation, which is a known equation that shows the relationship between the glass transition temperature of a polymer and the glass transition temperature Tg of a homopolymer of the monomers that make up that polymer.
[0066] The method for producing the (meth)acrylic resin is not particularly limited, and known methods can be used. For example, the above-mentioned acrylic raw material monomer components are contacted with a known polymerization initiator (such as a peroxide) under high temperature and high pressure conditions. This results in an anionic group-containing (meth)acrylic resin being obtained as a polymerization product of the acrylic raw material monomer components.
[0067] [Sealing Resin] The sealing resin may contain other resins as optional components. The other resins are resins other than polyolefin resins and (meth)acrylic resins. Examples of the other resins include polyester resins, polyamide resins, polyvinyl resins, polycarbonate resins, and cellulose resins. These may be used alone or in combination of two or more.
[0068] The filling resin preferably does not contain any other resins and is made of a polyolefin resin and a (meth)acrylic resin.
[0069] In the sealing resin, the ratio of the polyolefin resin to the (meth)acrylic resin is adjusted from the viewpoint of achieving a balance between the handleability (blocking resistance) and flex resistance of the sealing layer 3 .
[0070] More specifically, the content of the polyolefin resin relative to the total amount of the polyolefin resin and the (meth)acrylic resin is, for example, 6% by mass or more, preferably 20% by mass or more, more preferably 40% by mass or more, even more preferably 50% by mass or more, even more preferably more than 50% by mass, even more preferably 60% by mass or more, even more preferably 70% by mass or more, and particularly preferably 75% by mass or more. Also, the content of the polyolefin resin relative to the total amount of the polyolefin resin and the (meth)acrylic resin is, for example, 94% by mass or less, preferably 92% by mass or less, more preferably 90% by mass or less, even more preferably 88% by mass or less, and particularly preferably 85% by mass or less.
[0071] The content of the (meth)acrylic resin relative to the total amount of the polyolefin resin and the (meth)acrylic resin is, for example, 6% by mass or more, preferably 8% by mass or more, more preferably 10% by mass or more, even more preferably 12% by mass or more, and particularly preferably 15% by mass or more. The content of the (meth)acrylic resin relative to the total amount of the polyolefin resin and the (meth)acrylic resin is, for example, 94% by mass or less, preferably 80% by mass or less, more preferably 60% by mass or less, even more preferably 50% by mass or less, even more preferably less than 50% by mass, even more preferably 40% by mass or less, even more preferably 30% by mass or less, and particularly preferably 25% by mass or less.
[0072] When the ratio of the polyolefin resin to the (meth)acrylic resin is within the above range, the sealing layer 3 has particularly good handling properties (blocking resistance) and bending resistance.
[0073] [Method for producing seal resin] The form of the seal resin is not particularly limited as long as it contains a polyolefin resin and a (meth)acrylic resin. For example, the seal resin may be a resin composition (mixed resin) containing a polyolefin resin and a (meth)acrylic resin. Alternatively, the seal resin may be a composite resin (polyolefin-(meth)acrylic composite resin) containing a polyolefin resin and a (meth)acrylic resin.
[0074] When the filling resin is a resin composition (mixed resin) containing a polyolefin resin and a (meth)acrylic resin, for example, the polyolefin resin and the (meth)acrylic resin are prepared separately.
[0075] More specifically, the polyolefin resin is prepared in a state of being dissolved and / or dispersed in a solvent. For example, the polyolefin resin is synthesized in the solvent by polymerizing olefin raw material monomer components in the solvent. This results in a dispersion of the polyolefin resin (polyolefin dispersion).
[0076] The solvent is not particularly limited, but examples thereof include water, methanol, ethanol, propanol, isopropanol, acetone, methyl ethyl ketone, ethyl acetate, tetrahydrofuran, and acetonitrile. These solvents can be used alone or in combination of two or more. The solids concentration of the sealing coating material is not particularly limited and can be appropriately set depending on the purpose and application.
[0077] The (meth)acrylic resin is prepared in a state of being dissolved and / or dispersed in a solvent. For example, the (meth)acrylic resin is synthesized in the solvent by polymerizing the acrylic raw material monomer components in the solvent. This results in a dispersion of the (meth)acrylic resin (acrylic emulsion).
[0078] In this method, for example, a dispersion of a polyolefin resin (polyolefin dispersion) and a dispersion of a (meth)acrylic resin (acrylic emulsion) are mixed together, and the mixing ratio is adjusted so that the mass ratio of the polyolefin resin to the (meth)acrylic resin falls within the above range.
[0079] This results in a resin composition (mixed resin) containing the polyolefin resin and the (meth)acrylic resin in the solvent, in other words, a solution and / or dispersion of the filling resin (mixed resin).
[0080] Furthermore, when the filling resin is a composite (composite resin) containing a polyolefin resin and a (meth)acrylic resin, examples of the composite (composite resin) include core-shell particles.
[0081] The core-shell particles are produced by a known method. More specifically, the method for producing the core-shell particles is not particularly limited, but for example, an acrylic raw material monomer component is polymerized in a dispersion (polyolefin dispersion) containing the above-mentioned polyolefin resin. The polymerization method is appropriately selected depending on the type and amount of the acrylic raw material monomer component.
[0082] As a result, the (meth)acrylic resin is synthesized in the above solvent so as to coat the polyolefin resin. After the reaction is completed, the (meth)acrylic resin is neutralized with a known neutralizing agent, if necessary.
[0083] As a result, core-shell particles having a core containing a polyolefin resin and a shell containing a (meth)acrylic resin covering the core are obtained as a composite resin. In other words, a solution and / or dispersion of a filling resin (composite resin) is obtained. Preferably, an emulsion of a polyolefin-(meth)acrylic composite resin is obtained.
[0084] The composite resin is not limited to the core-shell particles described above, and examples of the composite resin include core-shell particles having a core containing a (meth)acrylic resin and a shell covering the core and containing a polyolefin resin.
[0085] Furthermore, as the sealing resin, a resin composition (mixed resin) containing the above-mentioned polyolefin resin and (meth)acrylic resin and a composite resin (polyolefin-(meth)acrylic composite resin) containing a polyolefin resin and a (meth)acrylic resin can also be used in combination.
[0086] From the viewpoint of storage stability, the filling resin is preferably a composite resin containing a polyolefin resin and a (meth)acrylic resin (polyolefin-(meth)acrylic composite resin).
[0087] On the other hand, from the viewpoint of coating drying property, the sealing resin is preferably a resin composition (mixed resin) containing a polyolefin resin and a (meth)acrylic resin. That is, depending on the production method, the solid content concentration of the (meth)acrylic resin can be made relatively high. Therefore, the solid content concentration of the resin composition (mixed resin) containing a polyolefin resin and a (meth)acrylic resin can be made relatively high. Furthermore, a resin composition (mixed resin) having a relatively high solid content concentration has excellent coating drying property.
[0088] The solids concentration of the solution and / or dispersion of the filler resin is, for example, 10% by mass or more, preferably 15% by mass or more, more preferably 20% by mass or more, and for example, 60% by mass or less, preferably 50% by mass or less, more preferably 40% by mass or less.
[0089] [Sealing Coating Material] The sealing coating material contains a solution and / or dispersion of the sealing resin. That is, the sealing coating material contains the sealing resin and the solvent. Furthermore, the sealing coating material can contain additives as needed. That is, the sealing coating material can contain the sealing resin, additives, and solvent.
[0090] Examples of additives include heat stabilizers, antioxidants, light stabilizers, ultraviolet absorbers, plasticizers, antistatic agents, lubricants, antiblocking agents, pigments, dyes, nucleating agents, and curing agents. These can be used alone or in combination of two or more. The amount and timing of addition of the additives are appropriately determined depending on the purpose and application.
[0091] The solid content concentration of the filler coating material is, for example, 10% by mass or more, preferably 15% by mass or more, more preferably 20% by mass or more, and for example, 60% by mass or less, preferably 50% by mass or less, more preferably 40% by mass or less.
[0092] The method for applying the filler coating material is not particularly limited. Examples of application methods include dip coating, gravure coating, reverse coating, roll coating, bar coating, spray coating, and air knife coating. The drying conditions for the filler coating material are not particularly limited. For example, the drying temperature is, for example, 40°C or higher, preferably 50°C or higher. The drying temperature is, for example, 200°C or lower, preferably 180°C or lower. The drying time is, for example, 1 second or longer, preferably 30 seconds or longer. The drying time is, for example, 10 minutes or shorter, preferably 5 minutes or shorter.
[0093] This forms the filling layer 3. The amount (dry mass) of the filling layer 3 is, for example, 1 g / m 2 More than 3 g / m 2 The amount (dry mass) of the filling layer 3 is, for example, 30 g / m 2 Preferably, 15 g / m or less 2 The following is the result.
[0094] (3) Gas Barrier Layer The gas barrier layer 4 is a layer having gas barrier properties. Gas barrier properties are the property of reducing oxygen permeability. More specifically, the gas barrier layer 4 is made of a gas barrier resin having an oxygen permeability of a predetermined value or less. For example, the oxygen permeability of a gas barrier layer 4 having a thickness of 10 μm is, for example, 1 (cc / m) at room temperature. 2·day·atm) or less. The oxygen permeability is measured in accordance with JIS K7126 (2006) Method B using an oxygen permeability measuring device (MOCON, OX-TRAN2 / 22H). The measurement conditions are 20°C and 80% RH (relative humidity).
[0095] The gas barrier layer 4 is disposed on the surface of the filling layer 3. That is, the gas barrier layer 4 is disposed on the surface of the filling layer 3 on the side of the paper base material 2 on which the filling layer 3 is disposed. The gas barrier layer 4 may be disposed on both sides of the paper base material 2 together with the filling layer 3. The gas barrier layer 4 is preferably disposed on only one surface of the paper base material 2 together with the filling layer 3.
[0096] Examples of the gas barrier layer 4 include inorganic layers and resin layers. The inorganic layer contains, for example, a metal and / or a metal oxide. Examples of the metal include aluminum. Examples of the metal oxide include aluminum oxide and silicon oxide. More specifically, examples of the inorganic layer include a metal thin film layer and a metal vapor deposition layer. The resin layer contains, for example, a gas barrier resin. More specifically, examples of the resin layer include a barrier coat layer and a barrier film layer.
[0097] The gas barrier layer 4 is preferably a barrier coating layer containing a gas barrier resin. More specifically, the gas barrier layer 4 is formed, for example, by applying a coating material containing a gas barrier resin (hereinafter, referred to as a gas barrier coating material) to the filling layer 3 and drying the coating material.
[0098] The gas barrier resin is a resin having an oxygen permeability of a predetermined value or less. More specifically, the oxygen permeability of a 10 μm thick film made of a gas barrier resin is, for example, 1 (cc / m) at room temperature. 2 ·day·atm) or less. The oxygen permeability is measured in accordance with JIS K7126 (2006) Method B using an oxygen permeability measuring device (MOCON, OX-TRAN2 / 22H). The measurement conditions are 20°C and 80% RH (relative humidity).
[0099] The gas barrier resin is not particularly limited. Examples of the gas barrier resin include a gas barrier polyurethane resin and a gas barrier acrylic resin. These can be used alone or in combination of two or more. From the viewpoint of gas barrier properties, a gas barrier polyurethane resin is preferably used as the gas barrier resin. That is, the gas barrier resin preferably contains a gas barrier polyurethane resin, and more preferably consists of a gas barrier polyurethane resin.
[0100] The gas barrier polyurethane resin is a resin having an oxygen permeability equal to or less than the above-mentioned predetermined value. The gas barrier polyurethane resin is not particularly limited, and a known gas barrier polyurethane resin can be used. For example, the gas barrier polyurethane resin is contained in a polyurethane dispersion (PUD) as a gas barrier coating material.
[0101] The gas barrier polyurethane resin and the polyurethane dispersion are produced, for example, in accordance with the description of paragraphs
[0026] to
[0111] of JP 2015-044396 A and paragraphs
[0048] to
[0141] of JP 2021-115802 A.
[0102] More specifically, the gas barrier polyurethane resin contains, for example, a reaction product of an isocyanate-terminated prepolymer and a chain extender, preferably a reaction product of an isocyanate-terminated prepolymer and a chain extender. The isocyanate-terminated prepolymer contains, for example, a reaction product of a polyisocyanate component and an active hydrogen group-containing component, preferably a reaction product of a polyisocyanate component and an active hydrogen group-containing component.
[0103] That is, the primary reaction product of the polyisocyanate component and the active hydrogen group-containing component is an isocyanate-terminated prepolymer, and the secondary reaction product of the isocyanate-terminated prepolymer and the chain extender is a gas-barrier polyurethane resin.
[0104] Examples of the polyisocyanate component include known polyisocyanate components. From the viewpoint of gas barrier properties, the polyisocyanate component preferably contains xylylene diisocyanate and / or hydrogenated xylylene diisocyanate. Furthermore, the polyisocyanate component may contain other polyisocyanates (polyisocyanates excluding xylylene diisocyanate and hydrogenated xylylene diisocyanate) as needed. Examples of other polyisocyanates include polyisocyanates commonly used industrially. More specific examples of other polyisocyanates include pentamethylene diisocyanate (PDI), hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), norbornene diisocyanate (NBDI), methylenebis(cyclohexyl isocyanate) (H 12 Examples of the polyisocyanate include diphenylmethane diisocyanate (MDI), tolylene diisocyanate (TDI), toluidine diisocyanate (TODI), naphthalene diisocyanate (NDI), and tetramethylxylylene diisocyanate (TMXDI). These may be used alone or in combination of two or more. Other preferred polyisocyanates include methylenebis(cyclohexyl isocyanate) (H 12 MDI). The polyisocyanate component may be a monomer or a derivative. Examples of the derivative include a polymer, an isocyanurate-modified product, an allophanate-modified product, a polyol adduct, a biuret-modified product, a urea-modified product, an oxadiazinetrione-modified product, and a carbodiimide-modified product. These may be used alone or in combination of two or more types.
[0105] The polyisocyanate component preferably contains xylylene diisocyanate and / or hydrogenated xylylene diisocyanate and another polyisocyanate (preferably methylenebis(cyclohexylisocyanate)). The content ratio of these components is appropriately set depending on the purpose and application.
[0106] The active hydrogen group-containing component is an organic compound containing an active hydrogen group. Examples of the active hydrogen group include a hydroxyl group and an amino group, and preferably a hydroxyl group. Examples of the active hydrogen group-containing component include known active hydrogen group-containing compounds. From the viewpoint of gas barrier properties, the active hydrogen group-containing component preferably contains a short-chain diol having 2 to 6 carbon atoms and an active hydrogen group-containing compound containing an anionic group.
[0107] The short-chain diol having 2 to 6 carbon atoms is an organic compound having 2 to 6 carbon atoms and two hydroxyl groups per molecule. Examples of short-chain diols include alkanediols having 2 to 6 carbon atoms and etherdiols having 2 to 6 carbon atoms, preferably alkanediols having 2 to 6 carbon atoms. Examples of alkanediols having 2 to 6 carbon atoms include ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butylene glycol, 1,3-butylene glycol, 1,2-butylene glycol, 1,5-pentanediol, 1,6-hexanediol, and neopentyl glycol. These can be used alone or in combination of two or more. From the viewpoint of gas barrier properties, ethylene glycol is preferred.
[0108] As the active hydrogen group-containing compound containing an anionic group, preferably, an organic compound having one carboxy group and two or more hydroxyl groups in one molecule is used, and more preferably, an organic compound having one carboxy group and two hydroxyl groups in one molecule is used. Examples of organic compounds having one carboxy group and two hydroxyl groups in one molecule include carboxy group-containing diols. Examples of carboxy group-containing diols include dihydroxyalkanoic acids. Examples of dihydroxyalkanoic acids include 2,2-dimethylolacetic acid, 2,2-dimethylollactic acid, 2,2-dimethylolpropionic acid (also known as dimethylolpropionic acid), 2,2-dimethylolbutanoic acid, 2,2-dimethylolbutyric acid, and 2,2-dimethylolvaleric acid. These can be used alone or in combination of two or more. From the viewpoint of water dispersibility, 2,2-dimethylolpropionic acid is preferred.
[0109] In the active hydrogen group-containing component, the content of the short-chain diol having 2 to 6 carbon atoms and the content of the active hydrogen group-containing compound having an anionic group are appropriately set depending on the purpose and application.
[0110] The active hydrogen group-containing component can further contain other polyols. Examples of other polyols include low-molecular-weight polyols with trihydric or higher hydricity, short-chain diols with 7 or more carbon atoms, and high-molecular-weight polyols. These can be used alone or in combination of two or more. Preferred examples of other polyols include low-molecular-weight polyols with trihydric or higher hydricity, and preferably trihydric alcohols and tetrahydric alcohols. Examples of trihydric alcohols include glycerin, 2-methyl-2-hydroxymethyl-1,3-propanediol, 2,4-dihydroxy-3-hydroxymethylpentane, 1,2,6-hexanetriol, trimethylolpropane, and 2,2-bis(hydroxymethyl)-3-butanol. Examples of tetrahydric alcohols include tetramethylolmethane (pentaerythritol) and diglycerin. These can be used alone or in combination of two or more. More preferred examples of low-molecular-weight polyols with trihydric or higher hydricity include trihydric alcohols, and even more preferred examples include trimethylolpropane. In addition, as the other polyol, for example, an active hydrogen group-containing compound containing a nonionic group can be mentioned. The active hydrogen group-containing compound containing a nonionic group can be used together with the above-mentioned active hydrogen compound containing an anionic group. In addition, the active hydrogen group-containing compound containing a nonionic group can be used instead of the above-mentioned active hydrogen compound containing an anionic group. In the active hydrogen group-containing component, the content ratio of the other polyol can be appropriately set according to the purpose and application.
[0111] The method for synthesizing the isocyanate-terminated prepolymer is not particularly limited. For example, the above-mentioned components are mixed in a predetermined equivalent ratio and reacted. Examples of the reaction method include bulk polymerization and solution polymerization, and solution polymerization is preferred. In the above reaction, a urethane catalyst can be added in an appropriate ratio as needed.
[0112] Furthermore, when the isocyanate group-terminated prepolymer has an anionic group derived from an active hydrogen compound containing an anionic group, the isocyanate group-terminated prepolymer is neutralized with a known neutralizing agent (e.g., triethylamine) to form a salt of the anionic group.
[0113] The isocyanate group concentration of the isocyanate group-terminated prepolymer is, for example, 4% by mass or more, preferably 5% by mass or more, more preferably 6% by mass or more, and for example, 25% by mass or less, preferably 20% by mass or less, more preferably 17% by mass or less, and even more preferably 15% by mass or less.
[0114] Next, in this method, the isocyanate-terminated prepolymer (primary reaction product) is reacted with a chain extender to obtain a gas-barrier polyurethane resin (secondary reaction product). For example, by reacting the isocyanate-terminated prepolymer with the chain extender in water, the gas-barrier polyurethane resin is produced and dispersed in water.
[0115] The chain extender is an organic compound that causes a chain extension reaction of the isocyanate-terminated prepolymer. The chain extender has multiple active hydrogen groups. Examples of the chain extender include polyamines, amino-group-containing alkoxysilyl compounds, and amino alcohols (e.g., 2-((2-aminoethyl)amino)ethanol).
[0116] The method for reacting the isocyanate-terminated prepolymer with the chain extender in water is not particularly limited. For example, the isocyanate-terminated prepolymer is first dispersed in water. Next, the chain extender is added to the water in which the isocyanate-terminated prepolymer is dispersed, and the isocyanate-terminated prepolymer is chain-extended in water. In this method, water can be added after completion of the reaction to adjust the solids concentration.
[0117] The chain extension reaction described above produces an aqueous dispersion of a gas-barrier polyurethane resin (hereinafter referred to as a primary polyurethane dispersion, or primary PUD). The primary polyurethane dispersion (primary PUD) is an aqueous dispersion containing a gas-barrier polyurethane resin but not containing the additives described below.
[0118] The gas barrier resin is not limited to the above gas barrier polyurethane resin, and is preferably prepared as an aqueous dispersion (primary aqueous dispersion) of the gas barrier resin.
[0119] The solid content concentration of the aqueous dispersion (primary aqueous dispersion) of the gas barrier resin is, for example, 10% by mass or more, preferably 15% by mass or more, and more preferably 20% by mass or more. The solid content concentration of the aqueous dispersion (primary aqueous dispersion) of the gas barrier resin is, for example, 60% by mass or less, preferably 50% by mass or less, and more preferably 40% by mass or less.
[0120] The aqueous dispersion (primary aqueous dispersion) of the gas barrier resin can be used as it is as a gas barrier coating material. That is, the gas barrier coating material can be made of, for example, the aqueous dispersion (primary aqueous dispersion) of the gas barrier resin.
[0121] The gas barrier coating material may contain an additive. Preferably, the gas barrier coating material contains an additive. That is, preferably, an aqueous dispersion (secondary aqueous dispersion) containing the gas barrier resin and the additive is used as the gas barrier coating material.
[0122] Examples of additives include layered inorganic compounds, thickening inhibitors, heat stabilizers, antioxidants, light stabilizers, UV absorbers, plasticizers, antistatic agents, lubricants, antiblocking agents, pigments, dyes, nucleating agents, and curing agents. These can be used alone or in combination of two or more. From the viewpoint of gas barrier properties, layered inorganic compounds are preferred as additives. That is, the gas barrier layer 4 preferably contains a layered inorganic compound. The amount and timing of addition of the additives are appropriately determined depending on the purpose and application.
[0123] The solid content concentration of the gas barrier coating material is, for example, 10% by mass or more, preferably 15% by mass or more, more preferably 20% by mass or more, and for example, 60% by mass or less, preferably 50% by mass or less, more preferably 40% by mass or less.
[0124] The method for applying the gas barrier coating material is not particularly limited. Examples of application methods include dip coating, gravure coating, reverse coating, roll coating, bar coating, spray coating, and air knife coating. The drying conditions for the gas barrier coating material are not particularly limited. For example, the drying temperature is, for example, 40°C or higher, preferably 50°C or higher. The drying temperature is, for example, 200°C or lower, preferably 180°C or lower. The drying time is, for example, 1 second or longer, preferably 30 seconds or longer. The drying time is, for example, 10 minutes or shorter, preferably 5 minutes or shorter.
[0125] This forms the gas barrier layer 4. The amount (dry mass) of the gas barrier layer 4 is, for example, 0.1 g / m 2 More than 0.2 g / m 2 The amount (dry mass) of the gas barrier layer 4 is, for example, 10 g / m 2 Preferably, 7 g / m or less 2 The following is the result.
[0126] (4) Heat-seal layer The heat-seal layer 5 is a resin layer with heat-sealing properties. The heat-seal layer 5 is disposed on the surface of the gas barrier layer 4. That is, the heat-seal layer 5 is disposed on the surface of the gas barrier layer 4 on the side of the paper base material 2 on which the gas barrier layer 4 is disposed. The heat-seal layer 5 may be disposed on both sides of the paper base material 2 together with the gas barrier layer 4. The heat-seal layer 5 is preferably disposed on only one surface of the paper base material 2 together with the gas barrier layer 4.
[0127] The heat seal layer 5 contains, for example, a heat sealable resin. More specifically, the heat seal layer 5 is formed, for example, by applying a coating material containing a heat sealable resin (hereinafter referred to as a heat sealable coating material) to the gas barrier layer 4 and drying it.
[0128] Heat-sealable resins are resins that can be heat-sealed (thermally fused) to each other. There are no particular limitations on the heat-sealable resin, and known heat-sealable resins can be used. More specific examples of heat-sealable resins include polyolefin resins, acrylic resins, and polyurethane resins. Examples of heat-sealable resins include resin compositions (mixed resins) containing polyolefin resins and (meth)acrylic resins. Examples of heat-sealable resins include composite resins containing polyolefin resins and (meth)acrylic resins (polyolefin-(meth)acrylic composite resins). The heat-sealable resin may be the same as the sealing resin. These can be used alone or in combination of two or more types. Examples of heat-sealable resins include preferably polyolefin resins and (meth)acrylic resins, more preferably a single polyolefin resin or a combination of polyolefin resins and (meth)acrylic resins, even more preferably a combination of polyolefin resins and (meth)acrylic resins, and particularly preferably a composite resin containing polyolefin resins and (meth)acrylic resins (polyolefin-(meth)acrylic composite resins). The heat-sealable resin is preferably the same as the sealing resin.
[0129] The heat-sealable resin is prepared, for example, as a solution and / or dispersion in which it is dissolved and / or dispersed in a solvent. For example, the heat-sealable resin is synthesized in a solvent. This results in a solution and / or dispersion of the heat-sealable resin.
[0130] The solvent is not particularly limited, but examples thereof include water, methanol, ethanol, propanol, isopropanol, acetone, methyl ethyl ketone, ethyl acetate, tetrahydrofuran, and acetonitrile. These solvents can be used alone or in combination of two or more. The solids concentration of the sealing coating material is not particularly limited and can be appropriately set depending on the purpose and application.
[0131] More specifically, examples of the heat-sealable coating material include a polyolefin dispersion containing a polyolefin resin, an acrylic emulsion containing an acrylic resin, and a polyurethane dispersion containing a polyurethane resin. A preferred example of the heat-sealable coating material is a polyolefin dispersion.
[0132] The heat-sealable coating material can contain additives. That is, the heat-sealable coating material can contain the above-mentioned heat-sealable resin and additives. Examples of additives include heat stabilizers, antioxidants, light stabilizers, ultraviolet absorbers, plasticizers, antistatic agents, lubricants, antiblocking agents, pigments, dyes, nucleating agents, and curing agents. These can be used alone or in combination of two or more.
[0133] The solid content concentration of the heat-sealable coating material is, for example, 10% by mass or more, preferably 15% by mass or more, more preferably 20% by mass or more, and for example, 60% by mass or less, preferably 50% by mass or less, more preferably 40% by mass or less.
[0134] The application method of the heat-sealable coating material is not particularly limited. Examples of application methods include dip coating, gravure coating, reverse coating, roll coating, bar coating, spray coating, and air knife coating. The drying conditions of the gas barrier coating material are not particularly limited. For example, the drying temperature is, for example, 40°C or higher, preferably 50°C or higher. The drying temperature is, for example, 200°C or lower, preferably 180°C or lower. The drying time is, for example, 1 second or longer, preferably 30 seconds or longer. The drying time is, for example, 10 minutes or shorter, preferably 5 minutes or shorter.
[0135] This forms the heat seal layer 5. The amount (dry mass) of the heat seal layer 5 is set from the viewpoint of achieving both gas barrier properties and heat sealability.
[0136] More specifically, from the viewpoint of heat sealing property, the amount (dry mass) of the heat seal layer 5 is, for example, 1.0 g / m 2 More than 1.0 g / m 2 More preferably, 1.1 g / m 2 More preferably, 1.5 g / m 2 More preferably, 1.8 g / m 2 From the viewpoint of gas barrier properties, the amount (dry mass) of the heat seal layer 5 is, for example, 7.0 g / m 2 Preferably, 5.0 g / m or less 2 less than 4.9 g / m 2 More preferably, 4.0 g / m 2 Below, particularly preferably 3.5 g / m 2 The following is the result.
[0137] (5) Laminate The laminate 1 has a total thickness of, for example, 5 μm or more, or preferably 10 μm or more. The laminate 1 has a total thickness of, for example, 1 mm or less, or preferably 0.5 mm or less.
[0138] 2. Effects The laminate 1 includes a paper substrate 2, a sealing layer 3, and a gas barrier layer 4. In the laminate 1, the sealing layer 3 contains a polyolefin resin and a (meth)acrylic resin. Therefore, the sealing layer 3 has excellent blocking resistance. That is, the laminate 1 has excellent handleability. Furthermore, since the sealing layer 3 contains a polyolefin resin and a (meth)acrylic resin, it has excellent flex resistance. As a result, the laminate 1 has both excellent handleability and excellent flex resistance.
[0139] 3. Uses The laminate 1 is suitable for use in various industrial fields that require gas barrier properties and heat sealability. More specifically, the laminate 1 is suitable for use as a packaging material. That is, the packaging material preferably contains the laminate 1, and more preferably consists of the laminate 1.
[0140] Such a packaging material has excellent handling properties and excellent flex resistance because it contains the laminate 1. Such a packaging material is used in various industrial fields. Preferably, the packaging material is used in the food packaging field.
[0141] 4. Modifications The laminate 1 and packaging material described above include a heat seal layer 5. However, the heat seal layer 5 is an optional layer. In other words, the laminate 1 and packaging material may not include the heat seal layer 5 depending on the purpose and application.
[0142] Furthermore, when the laminate 1 and the packaging material include a heat seal layer 5, the heat seal layer 5 may be laminated directly on the gas barrier layer 4, as described above. Alternatively, the heat seal layer 5 may be bonded to the gas barrier layer 4 with a known adhesive. That is, an adhesive layer (not shown) may be interposed between the gas barrier layer 4 and the heat seal layer 5. Alternatively, instead of the heat seal layer 5, or together with the heat seal layer 5, an arbitrary functional layer may be laminated on the gas barrier layer 4.
[0143] Next, the present invention will be described based on examples and comparative examples, but the present invention is not limited to the following examples. Note that "parts" and "%" are by mass unless otherwise specified. Furthermore, specific numerical values such as blending ratios (content ratios), physical property values, parameters, etc. used in the following description can be substituted with the corresponding upper limit values (numeric values defined as "equal to or less than") or lower limit values (numeric values defined as "equal to or more than" or "exceeding") of the blending ratios (content ratios), physical property values, parameters, etc. described in the above "Modes for Carrying Out the Invention."
[0144] 1. Paper Base Preparation Example 1 The following papers were prepared as paper bases: (1) Gintake: One-sided gloss (unbleached) kraft paper, product name "Gintake", manufactured by Nippon Paper Industries Co., Ltd., basis weight 41.7 g / m 2 , 66.6 g / m 2 , 83.3 g / m 2 (2) Shirogane: One-sided gloss (bleached) kraft paper, product name "Shirogane", manufactured by Nippon Paper Industries Co., Ltd., basis weight 30 g / m 2 , 65 g / m 2 (3) Kinshachi: Pure white roll paper, product name "Kinshachi", manufactured by Daio Paper Co., Ltd., basis weight 30 g / m 2 , 65 g / m 2 (4) Nagoya Sarashi Ryuo: One-sided gloss (bleached) kraft paper, product name “Nagoya Sarashi Ryuo”, manufactured by Daio Paper Corporation, basis weight 60 g / m 2 (5) Glassine paper; product name “Thick white glassine”, manufactured by Nippon Paper Industries Co., Ltd., basis weight 30.5 g / m 2 (6) Coated paper; product name “N Coat Wrap L”, manufactured by Nippon Paper Industries Co., Ltd., basis weight 65 g / m 2 (7) Cup base paper: Product name “Cup base paper (uncoated product)”, manufactured by Nippon Paper Industries Co., Ltd., basis weight 150 g / m 2
[0145] 2. Gas Barrier Coating Material Synthesis Example 1 (Primary Polyurethane Dispersion) The following components were mixed and reacted in a nitrogen atmosphere at 65 to 70°C until the isocyanate group concentration (NCO%) reached 6.11% by mass or less, thereby obtaining a transparent isocyanate-terminated prepolymer reaction product liquid.
[0146] 1,3-xylylene diisocyanate (Takenate 500, 1,3-XDI, manufactured by Mitsui Chemicals, Inc.) 143.2 parts by mass Methylenebis(cyclohexyl isocyanate) (VestanatH 12 MDI, H 12 MDI (manufactured by Evonik) 25.0 parts by weight Ethylene glycol 29.2 parts by weight Trimethylolpropane 2.7 parts by weight Dimethylolpropionic acid 14.8 parts by weight Methyl ethyl ketone (solvent) 121.6 parts by weight
[0147] The reaction product liquid was then cooled to 40° C. Next, 11.0 parts by mass of triethylamine (TEA) was added to the reaction product liquid, thereby neutralizing the isocyanate-terminated prepolymer.
[0148] Next, the reaction product liquid was dispersed in 838.0 parts by mass of ion-exchanged water using a Homodisper. Next, an amine aqueous solution was added to the obtained dispersion liquid to carry out a chain extension reaction. The reaction product liquid of the chain extension reaction was aged for 1 hour. This resulted in a gas barrier polyurethane resin. The amine aqueous solution was a mixed liquid of 48.4 parts by mass of ion-exchanged water and 24.2 parts by mass of 2-((2-aminoethyl)amino)ethanol. Thereafter, methyl ethyl ketone and ion-exchanged water were distilled off from the reaction product liquid using an evaporator. This adjusted the solids concentration to 30% by mass.
[0149] As a result of the above, a primary polyurethane dispersion (primary PUD) in which the gas barrier polyurethane resin was dispersed in water was obtained.
[0150] The pH of the primary polyurethane dispersion (primary PUD) was 8.6. The average particle size of the polyurethane dispersion (primary PUD) was 58 nm. The average particle size was measured by dynamic light scattering (measurement device FPAR-1000, manufactured by Otsuka Electronics Co., Ltd.) (the same applies hereinafter).
[0151] Preparation Example 1 (Secondary Polyurethane Dispersion) A dispersion of a layered inorganic compound (product name: NTS-10NC, manufactured by Topy Industries, Ltd., solid content concentration 10.7%) (hereinafter referred to as synthetic mica 1) was prepared. The dispersion of the layered inorganic compound and water were mixed for 5 minutes. This resulted in a dispersion of an additive.
[0152] The primary PUD of Synthesis Example 1 and the dispersion of the additives were mixed for 5 minutes so that the solid mass ratio of the polyurethane resin to the layered inorganic compound (polyurethane resin:layered inorganic compound) was 5:15.
[0153] This resulted in a secondary polyurethane dispersion (secondary PUD) in which the gas barrier polyurethane resin and the additive (layered inorganic compound) were dispersed in water. The solids concentration of the secondary PUD was 15% by mass. This secondary PUD was used as gas barrier coating material 1.
[0154] Preparation Example 2 (Secondary Polyurethane Dispersion) A dispersion of a layered inorganic compound (product name: ME300-B4T, manufactured by Katakura Co-op Agri Co., Ltd., solid content concentration 7.8%) (hereinafter referred to as synthetic mica 2) was prepared.
[0155] A secondary polyurethane dispersion (secondary PUD) was obtained in the same manner as in Preparation Example 1, except that synthetic mica 2 was used instead of synthetic mica 1. The solids concentration of the secondary PUD was 15 mass %. The secondary PUD was used as gas barrier coating material 2.
[0156] Preparation Example 3 (Secondary Polyurethane Dispersion) A dispersion of a layered inorganic compound (trade name: Kunipia RC-I, Synthetic Mica 3, manufactured by Kunimine Industries Co., Ltd., solid content concentration 4.0%) was prepared.
[0157] A secondary polyurethane dispersion (secondary PUD) was obtained in the same manner as in Preparation Example 1, except that synthetic mica 3 was used instead of synthetic mica 1. The solids concentration of the secondary PUD was 15 mass %. The secondary PUD was used as gas barrier coating material 3.
[0158] Preparation Example 4 (PVA) Polyvinyl alcohol (trade name: Kuraray Poval PVA117, manufactured by Kuraray Co., Ltd.) (hereinafter referred to as PVA) was prepared. The PVA was dispersed in water. This resulted in an aqueous dispersion of PVA. The solid content of the aqueous dispersion of PVA was adjusted to 30% by mass.
[0159] A secondary polyurethane dispersion (secondary PUD) was obtained in the same manner as in Preparation Example 2, except that an aqueous dispersion of PVA was used instead of the primary PUD. The solids concentration of the secondary PUD was 15 mass%. The secondary PUD was used as a gas barrier coating material 4.
[0160] 3. Filler Coating Material Synthesis Example 2 (Polyolefin Dispersion (PO)) An ethylene-methacrylic acid copolymer (EMAA) was prepared as a polyolefin resin. The content of ethylene-derived structural units relative to the total amount of the ethylene-methacrylic acid copolymer was 80.0 mass %, and the content of methacrylic acid-derived structural units was 20.0 mass %.
[0161] 100 parts by mass of ethylene-methacrylic acid copolymer, 19.0 parts by mass of 15% aqueous ammonia, and 335 parts by mass of deionized water were stirred in a reaction vessel and maintained at 150°C for 4 hours. This resulted in the polyolefin resin being dispersed in water, yielding a polyolefin dispersion (PO; EMAA dispersion). The polyolefin dispersion (PO) had an average particle size (dynamic light scattering method) of 38 nm and a solids concentration of 22% by mass.
[0162] Synthesis Example 3 (Acrylic Emulsion (Ac)) 2,193 parts by mass of ion-exchanged water (solvent) and 2.5 parts by mass of sodium dodecyl sulfate (surfactant) were charged into a reaction vessel equipped with a stirrer, a reflux condenser, a dropping device, and a thermometer. The contents of the reaction vessel were heated to 75° C. while stirring and purging with nitrogen.
[0163] While maintaining the internal temperature of the reaction vessel at 75° C., 12.5 parts by mass of potassium persulfate (polymerization initiator) was added to the reaction vessel and dissolved in the contents of the reaction vessel. Thereafter, a monomer emulsion prepared in advance was continuously added dropwise to the reaction vessel over a period of 5 hours.
[0164] The monomer emulsion is a raw material composition containing the following components: 900 parts by mass of ion-exchanged water (solvent), 5 parts by mass of sodium dodecyl sulfate (surfactant), 1608 parts by mass of 2-ethylhexyl acrylate (raw material monomer), and 893 parts by mass of styrene (raw material monomer).
[0165] After the dropwise addition of the monomer emulsion was completed, the contents of the reaction vessel were aged for 3 hours. This allowed the raw material monomers to polymerize, yielding a (meth)acrylic resin. Also, an acrylic emulsion in which the (meth)acrylic resin was dispersed in water was obtained.
[0166] The acrylic emulsion was cooled to room temperature, and then ion-exchanged water and ammonia water (neutralizer) were added to the acrylic emulsion to adjust the solid content to 42% by mass and the pH to 8.0.
[0167] This resulted in an acrylic emulsion (Ac) in which the (meth)acrylic resin was dispersed in water. The average particle size of the acrylic emulsion was 257 nm.
[0168] The theoretical glass transition temperature of the (meth)acrylic resin was calculated based on the Fox formula and was found to be −30° C.
[0169] Synthesis Example 4 (Polyolefin-(meth)acrylic composite resin emulsion) A reaction vessel equipped with a stirrer, a reflux condenser, a dropping device, and a thermometer was charged with 1,031.6 parts by mass of polyolefin dispersion (PO). The contents of the reaction vessel were heated to 75°C while stirring and purging with nitrogen.
[0170] While maintaining the internal temperature of the reaction vessel at 75° C., 0.13 parts by mass of sodium persulfate (polymerization initiator) was added to the reaction vessel and dissolved in the contents of the reaction vessel. Thereafter, a previously prepared monomer emulsion was continuously added dropwise to the reaction vessel over a period of 5 hours.
[0171] The monomer emulsion is a raw material composition containing the following components: 20 parts by mass of ion-exchanged water (solvent), 0.05 parts by mass of sodium dodecyl sulfate (surfactant), 16.1 parts by mass of 2-ethylhexyl acrylate (raw material monomer), and 8.9 parts by mass of styrene (raw material monomer).
[0172] After the dropwise addition of the monomer emulsion was completed, the contents of the reaction vessel were aged for 3 hours. As a result, the raw material monomers were polymerized in the polyolefin dispersion (PO), and a (meth)acrylic resin (Ac) was synthesized. As a result, a polyolefin-(meth)acrylic composite resin (PO / Ac) was obtained. In addition, a composite resin emulsion in which the polyolefin-(meth)acrylic composite resin (PO / Ac) was dispersed in water was obtained.
[0173] The polyolefin-(meth)acrylic composite resin (PO / Ac) had a core-shell structure. In the core-shell structure, the core was the polyolefin resin (PO) and the shell was the (meth)acrylic resin (Ac). The glass transition temperature (Fox equation) of the (meth)acrylic resin contained in the polyolefin-(meth)acrylic composite resin (PO / Ac) was −30° C.
[0174] The composite resin emulsion was cooled to room temperature, and then ion-exchanged water was added to the composite resin emulsion to adjust the solid content to 25% by mass and the pH to 10.0.
[0175] This resulted in a composite resin emulsion in which polyolefin-(meth)acrylic composite resin (PO / Ac) was dispersed in water. The composite resin emulsion had an average particle size of 73 nm. The composite resin emulsion (solid content concentration: 25% by mass) was used as a sealing coating material.
[0176] Synthesis Examples 5 to 30 (Polyolefin-(meth)acrylic composite resin emulsions) The formulation of the monomer emulsion was changed to the formulations shown in Tables 1 to 3. Other than this, a composite resin emulsion in which a polyolefin-(meth)acrylic composite resin was dispersed in water was obtained in the same manner as in Synthesis Example 4. The composite resin emulsion (solid content concentration 25% by mass) was used as a sealing coating material. The glass transition temperature (Fox equation) of the (meth)acrylic resin in each formulation is shown in Tables 1 to 3.
[0177] Mixing Preparation Examples 1 to 9 (Mixed Resins) The polyolefin dispersion (EMAA dispersion) of Synthesis Example 1 and the acrylic emulsion of Synthesis Example 3 were mixed according to the formulation shown in Table 4. Ion-exchanged water was added to these mixtures to adjust the solids concentration to 25% by mass. This resulted in a mixed solution (Po+Ac) containing a polyolefin resin and a (meth)acrylic resin. The mixed solution (Po+Ac) containing a polyolefin resin and a (meth)acrylic resin was used as a sealing coating material.
[0178] 4. Heat-sealable coating material Preparation example 2 (HS-POD) A dispersion of a polyolefin resin having heat-sealability (HS) (product name: Chemipearl S500NW, manufactured by Mitsui Chemicals) (hereinafter referred to as HS-POD) was prepared. HS-POD was used as a heat-sealable coating material.
[0179] Preparation Example 3 (HS-POF) A polyolefin resin film having heat sealability (HS) (product name: HC-40, thickness 40 μm, manufactured by Mitsui Chemicals Tohcello Co., Ltd.) (hereinafter referred to as HS-POF) was prepared. The POF was used as a heat seal layer.
[0180] 5. Laminates Examples 1 to 57 and Comparative Examples 1 to 3 (Laminates) The sealing coating material was applied to one side (smooth side or non-smooth side) of a paper substrate using a bar coater in the combinations shown in Tables 5 to 12. The dry mass was the amount (g / m) shown in Tables 5 to 10. 2 The coating amount was adjusted so that the coating film of the filler coating material was 100%. Then, the coating film of the filler coating material was dried at 120°C for 60 seconds. In this way, a filler layer was formed.
[0181] Next, a gas barrier coating material was applied to the surface of the filling layer using a bar coater in the combinations shown in Tables 5 to 12. The dry mass was the amount (g / m) shown in Tables 5 to 12. 2 The coating amount was adjusted so that the coating film of the gas barrier coating material was 100%. Next, the coating film of the gas barrier coating material was dried at 120°C for 60 seconds. In this way, a gas barrier layer was formed on the surface of the filling layer. In this way, a laminate was obtained. The layer structure of the laminate was as follows:
[0182] Paper base material / filler layer / gas barrier layer
[0183] In addition, in Examples 10, 56, and 57, a heat-sealable coating material was applied to the surface of the gas barrier layer using a bar coater. In Example 10, the HS-POD of Preparation Example 2 was used as the heat-sealable coating material. In Example 56, the polyolefin-(meth)acrylic composite resin emulsion of Synthesis Example 6 was used as the heat-sealable coating material. In Example 57, the acrylic emulsion of Synthesis Example 3 was used as the heat-sealable coating material. In Examples 10, 56, and 57, the dry mass was 3 g / m 2 The amount of the heat-sealable coating material applied was adjusted so that the coating film of the heat-sealable coating material was 0.01g / m². The coating film of the heat-sealable coating material was then dried at 120°C for 60 seconds. This resulted in a heat-sealable layer being formed on the surface of the gas barrier layer. This resulted in a laminate. The layer structure of the laminate was as follows:
[0184] Paper base material / Sealing layer / Gas barrier layer / Heat seal layer
[0185] In Example 11, a heat-sealable film was attached to the surface of the gas barrier layer using an adhesive (product name A-616 / product name A-65 (manufactured by Mitsui Chemicals)). The adhesive was then cured at 40°C for 2 days. This resulted in a laminate. The layer structure of the laminate was as follows:
[0186] Paper base material / Sealing layer / Gas barrier layer / Adhesive layer / Heat seal layer
[0187] 6. Evaluation (1) Oxygen transmission rate (OTR) of laminate The oxygen transmission rate (cc / m) of the laminate before bending2 The oxygen permeability (per 1000 kJ / day atm) was measured using an oxygen permeability measuring device (MOCON, OX-TRAN 2 / 22H). The measurement temperature was 20°C. The relative humidity was 80% RH.
[0188] At 25°C, the laminate was heated at 2 kg / cm with the coated surface (the sealing layer and the gas barrier layer) facing inward. 2 The folding direction was changed by 90° so as to form a cross crease, and the laminate was again folded at a pressure of 2 kg / cm for 10 seconds. 2 The sheet was folded at a pressure of 0.05 for 10 seconds.
[0189] The oxygen permeability (cc / m) of the laminate after folding was 2 The results are shown in Tables 5 to 12.
[0190] (2) Water Vapor Transmission Rate (WVTR) of Laminate: The water vapor transmission rate (g / m) of the laminate before folding 2 The water vapor transmission rate (day) was measured using a water vapor transmission rate measuring device (MOCON, PARMATRAN-W 3 / 34 G). The measurement temperature was 40°C and the relative humidity was 90% RH.
[0191] At 25°C, the laminate was heated at 2 kg / cm with the coated surface (the sealing layer and the gas barrier layer) facing inward. 2 The folding direction was changed by 90° so as to form a cross crease, and the laminate was again folded at a pressure of 2 kg / cm for 10 seconds. 2 The sheet was folded at a pressure of 0.05 for 10 seconds.
[0192] The water vapor permeability (g / m) of the laminate after folding was 2 The results are shown in Tables 5 to 12.
[0193] (3) Blocking Resistance A laminate (a two-layer structure consisting of a paper substrate and a sealing layer) was prepared before the formation of the gas barrier layer. The sealing layer of the two-layer structure was pressed onto the printed surface of a paper packaging material (Kit Kat Biscuit Flavor (product name), manufactured by Nestle) using a heat sealer. The pressing temperature was 30°C and the pressing force was 0.5 kg / cm. 2The pressure bonding time was 10 seconds. After pressure bonding, the blocking resistance of the filling layer was evaluated according to the following criteria. The results are shown in Tables 5 to 12.
[0194] 5: The two-layered body and the paper packaging material did not stick together. 4: The two-layered body and the paper packaging material stuck together, but they peeled off naturally. 3: The two-layered body and the paper packaging material stuck together, but when they were peeled off by hand, no cohesive failure or ink transfer was observed. 2: The two-layered body and the paper packaging material stuck together. When they were peeled off by hand, cohesive failure or ink transfer was observed. 1: The two-layered body and the paper packaging material stuck together. When they were peeled off by hand, the paper substrate was destroyed.
[0195] (4) Storage Stability of Filler Coating Material Immediately after production of the filler coating material, the viscosity of the filler coating material at 25°C was measured under the following conditions. Measurement method: Apparent viscosity measurement method using a Brookfield rotational viscometer. Apparatus: B-type viscometer (model RB-85), manufactured by Toki Sangyo Co., Ltd. Rotor: No. 2 Rotation speed: 60 rpm
[0196] The sealant coating material was stored for two weeks at 60° C. After storage, the viscosity of the sealant coating material at 25° C. was measured under the above conditions.
[0197] The viscosity increase rate due to storage was calculated using the following formula. The results are shown in Tables 5 to 12. Viscosity increase rate (%) = [viscosity after storage / viscosity before storage] x 100
[0198]
[0199]
[0200]
[0201]
[0202]
[0203]
[0204]
[0205]
[0206]
[0207]
[0208]
[0209]
[0210] The above invention is provided as an exemplary embodiment of the present invention, but it is merely an example and should not be interpreted as being limiting. Modifications of the present invention that are obvious to those skilled in the art are intended to be included in the scope of the following claims.
[0211] The laminate and packaging material of the present invention are suitable for use in the food packaging field.
[0212] REFERENCE SIGNS LIST 1 laminate 2 substrate 3 sealing layer 4 gas barrier layer 5 heat seal layer
Claims
1. A laminate comprising: a paper base material; a filling layer disposed on at least one side of the paper base material; and a gas barrier layer disposed on at least one side of the filling layer, wherein the filling layer contains a polyolefin resin and a (meth)acrylic resin.
2. The laminate according to claim 1, wherein the content of said polyolefin resin is 6% by mass or more and 94% by mass or less, and the content of said (meth)acrylic resin is 6% by mass or more and 94% by mass or less, based on the total amount of said polyolefin resin and said (meth)acrylic resin.
3. The laminate according to claim 1, wherein the (meth)acrylic resin has a glass transition temperature of -60°C or higher and 10°C or lower.
4. The laminate according to claim 1, wherein the gas barrier layer contains a gas barrier resin.
5. The laminate according to claim 4, wherein the gas barrier resin contains a gas barrier polyurethane resin.
6. The laminate according to claim 5, wherein the gas barrier polyurethane resin contains a reaction product of an isocyanate-terminated prepolymer and a chain extender, the isocyanate-terminated prepolymer contains a reaction product of a polyisocyanate component and an active hydrogen group-containing component, the polyisocyanate component contains xylylene diisocyanate and / or hydrogenated xylylene diisocyanate, and the active hydrogen group-containing component contains a short-chain diol having 2 to 6 carbon atoms and an active hydrogen compound containing an anionic group.
7. The laminate according to claim 4, wherein the gas barrier layer further contains a layered inorganic compound.
8. The laminate according to claim 1, further comprising a heat seal layer disposed on at least one side of said gas barrier layer.
9. A packaging material comprising the laminate according to claim 1.
Citation Information
Patent Citations
Laminate
JP2021115802A
Barrier paper
JP2022155999A
Special paper-plastic composite film for keeping freshness of fruits and vegetables at room temperature
CN103144845A
Polymeric materials and their use in multilayer products
JP1998500635A
Moistureproof packaging material
JP2001018332A
Cited By
Barrier laminate, package, and method for producing barrier laminate
JP2026087463A
Barrier laminate, packaging, and method for manufacturing a barrier laminate
JP7889683B2
JPWO2026094739A1
Barrier laminate, packaging body, and method for producing barrier laminate
WO2026094739A1
Barrier laminate, package, and method for producing barrier laminate
WO2026105538A1