Honeycomb filter
The honeycomb filter's robust collection layer, with specific oxide thickness and particle size relationships, addresses the trade-off between collection performance and pressure loss, ensuring effective particulate matter collection and structural integrity under stress.
Patent Information
- Application Number
- PCT/JP2024/010931
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional honeycomb filters face a trade-off between improved particulate matter collection performance and increased pressure loss, with collection layers prone to peeling off due to stress from vibration and thermal shock, especially when bonded with inadequate oxide thickness.
A honeycomb filter design featuring a collection layer with non-oxide particles bonded via an oxide, where the oxide thickness is 0.077 μm or more, and the average particle size of non-oxide particles satisfies the relationship R≦1.0609e^(4.7057×T), ensuring robust bonding and resistance to stress-induced peeling.
The filter achieves excellent collection performance while preventing the collection layer from peeling off under stress conditions, maintaining efficiency and reducing pressure loss.
Smart Images

Figure JP2024010931_03102024_PF_FP_ABST
Abstract
Description
Honeycomb Filter
[0001] The present invention relates to a honeycomb filter, and more particularly to a honeycomb filter having a trapping layer disposed on the surface of porous partition walls for trapping particulate matter.
[0002] In recent years, regulations regarding the removal of particulate matter contained in exhaust gas emitted from gasoline engines have become stricter worldwide, and honeycomb filters having a honeycomb structure are used as filters for removing particulate matter. Hereinafter, particulate matter may be referred to as "PM." PM is an abbreviation for "Particulate Matter."
[0003] For example, a honeycomb filter can include a honeycomb structure having porous partition walls that define a plurality of cells, and plugging portions that plug either end of the cells. Such a honeycomb filter is structured so that the porous partition walls function as a filter to remove PM. Specifically, PM-containing exhaust gas is introduced into the inlet end face of the honeycomb filter, and the PM is filtered by being captured by the porous partition walls. The purified exhaust gas is then discharged from the outlet end face of the honeycomb filter. In this manner, PM can be removed from the exhaust gas.
[0004] Conventionally, techniques have been proposed to improve the filtering performance of honeycomb filters, such as thickening the partition walls of a honeycomb structure or reducing the size of the pores formed in the partition walls. However, when filtering performance is improved using the techniques described above, there is a problem that PM (e.g., soot) tends to clog the pores formed in the partition walls, resulting in an increase in pressure loss of the honeycomb filter. In other words, the techniques described above are not effective solutions because the effect of improving filtering performance and the effect of suppressing an increase in pressure loss are in a trade-off relationship.
[0005] For this reason, a honeycomb filter has been proposed in which a trapping layer for trapping PM is disposed on the surface of the partition walls of a honeycomb structure (see, for example, Patent Document 1). For example, the trapping layer is formed of a porous membrane having an average pore diameter smaller than that of the partition walls. With such a honeycomb filter, PM can be deposited on the surface of the trapping layer, thereby improving the PM trapping efficiency while suppressing a sudden increase in pressure loss due to clogging of the pores of the partition walls with PM.
[0006] Japanese Patent Application Laid-Open No. 2012-206061
[0007] As described above, a honeycomb filter having a trapping layer on the surface of the partition walls is produced by forming a film of fine powder on a honeycomb filter precursor, which serves as a substrate, to form a dense film (i.e., a trapping layer) on the surface of the partition walls. Mainly used film-forming methods include filtering a solution containing a membrane material with a honeycomb filter precursor and drawing an aerosol containing a membrane material into the honeycomb filter precursor. In addition to the same material as the substrate, inorganic compounds such as metal oxides and metal carbides are also used for the membrane material. The process of bonding the membrane material to the substrate includes sintering by heat treatment or oxide film formation.
[0008] Conventionally, in the technology for forming a trapping layer, heat treatment has been performed to bond the above-mentioned membrane material, but the conditions that must be met to withstand various loads after installation in a vehicle have not been specified. For example, the above-mentioned Patent Document 1 characterizes the melting point of the membrane material bonding portion as being at least equal to or higher than the membrane material, but does not specify the structure of the bonding portion. When a honeycomb filter is installed and used in a vehicle, it is subjected to stresses such as vibration and thermal shock in addition to temperature. If the bonding portion of the membrane material is only formed very small, there is a concern that the structure of the trapping layer will be destroyed, even if the bonding portion has a high melting point. For example, the trapping layer may peel off from the partition wall when subjected to stresses such as vibration and thermal shock.
[0009] The present invention has been made in view of the problems associated with the conventional techniques, and provides a honeycomb filter in which the trapping layer is less likely to peel off from the partition walls even when subjected to stress such as vibration or thermal shock.
[0010] According to the present invention, there is provided the following honeycomb filter.
[0011] [1] A honeycomb structure having porous partition walls arranged to surround a plurality of cells that form fluid flow paths extending from an inflow end face to an outflow end face, and plugging portions arranged to plug either an end of the cells on the inflow end face side or the outflow end face side, wherein the plugging portions are arranged on the end of the outflow end face side and the cells that are open on the inflow end face side are inflow cells, and the plugging portions are arranged on the end of the inflow end face side and the cells that are open on the outflow end face side are outflow cells, and the honeycomb structure further has a collection layer for collecting particulate matter in exhaust gas on the inner surface side of the partition walls that surround the inflow cells, The trapping layer is a porous layer in which a plurality of non-oxide particles are bonded together via an oxide, and the thickness of the oxide bonding adjacent non-oxide particles is 0.077 μm or more. Furthermore, when the average particle size of the non-oxide particles constituting the trapping layer is R (μm) and the thickness of the oxide is T (μm), the relationship R≦1.0609e^(4.7057×T) is satisfied.
[0012] [2] The honeycomb filter according to [1], wherein the oxide constituting the trapping layer is disposed so as to cover the surfaces of the non-oxide particles.
[0013] [3] The honeycomb filter according to the above [1] or [2], wherein the non-oxide particles are silicon carbide particles.
[0014] The honeycomb filter of the present invention is a honeycomb filter having a trapping layer for trapping particulate matter in exhaust gas on the inner surface side of the partition walls surrounding the inlet cells, and has excellent trapping performance. The trapping layer is a porous layer in which a plurality of non-oxide particles are bonded together via an oxide, and the thickness of the oxide bonding adjacent non-oxide particles is 0.077 μm or more. Furthermore, this trapping layer satisfies the relationship R≦1.0609e^(4.7057×T), where R (μm) is the average particle size of the non-oxide particles constituting the trapping layer and T (μm) is the thickness of the oxide. Therefore, the trapping layer of the honeycomb filter of the present invention is less likely to break even when subjected to stress such as vibration or thermal shock, and peeling of the trapping layer from the partition walls can be effectively suppressed.
[0015] FIG. 2 is a perspective view schematically showing one embodiment of a honeycomb filter of the present invention. FIG. 3 is a plan view of the inflow end face side of the honeycomb filter shown in FIG. 1. FIG. 4 is a plan view of the outflow end face side of the honeycomb filter shown in FIG. 1. FIG. 5 is a cross-sectional view schematically showing the AA' cross section of FIG. 2. FIG. 6 is a cross-sectional view schematically showing a cross section of a partition wall. FIG. 7 is an enlarged cross-sectional view of the trapping layer in the range indicated by symbol P in FIG. 5. FIG. 8 is a schematic plan view for explaining the configuration of a vibration tester for performing a peeling test of the trapping layer.
[0016] While the present invention will be described below with reference to exemplary embodiments, it should be understood that the present invention is not limited to the following exemplary embodiments. Therefore, it should be understood that modifications and improvements to the following exemplary embodiments, based on the ordinary knowledge of those skilled in the art, are also within the scope of the present invention, provided that they do not deviate from the spirit of the present invention.
[0017] (1) Honeycomb filter: An embodiment of the honeycomb filter of the present invention is a honeycomb filter 100 as shown in Figs. 1 to 4. Here, Fig. 1 is a perspective view schematically showing one embodiment of the honeycomb filter of the present invention. Fig. 2 is a plan view of the inflow end face side of the honeycomb filter shown in Fig. 1. Fig. 3 is a plan view of the outflow end face side of the honeycomb filter shown in Fig. 1. Fig. 4 is a cross-sectional view schematically showing the A-A' cross section of Fig. 2.
[0018] As shown in Figures 1 to 4, a honeycomb filter 100 of this embodiment includes a honeycomb structure 4 and plugging portions 5. The honeycomb structure 4 has porous partition walls 1 arranged so as to surround a plurality of cells 2 that serve as fluid flow paths extending from an inflow end face 11 to an outflow end face 12. The honeycomb structure 4 shown in Figures 1 to 4 is configured in a cylindrical shape with the inflow end face 11 and the outflow end face 12 as both end faces, and further has an outer peripheral wall 3 on its outer peripheral side surface. That is, the outer peripheral wall 3 is arranged so as to surround the partition walls 1 arranged in a lattice pattern.
[0019] The plugging portions 5 are arranged so as to plug either one of the ends of the cells 2, on the inlet end face 11 side or the outlet end face 12 side. Hereinafter, among the plurality of cells 2, a cell 2 having a plugging portion 5 arranged at an end on the outlet end face 12 side and open on the inlet end face 11 side will be referred to as an "inlet cell 2a." Furthermore, among the plurality of cells 2, a cell 2 having a plugging portion 5 arranged at an end on the inlet end face 11 side and open on the outlet end face 12 side will be referred to as an "outlet cell 2b." In the honeycomb filter 100 of this embodiment, the inlet cells 2a and the outflow cells 2b are preferably arranged alternately with the partition wall 1 therebetween.
[0020] The honeycomb filter 100 is characterized in that the honeycomb structure 4 is configured as follows. That is, as shown in FIGS. 5 and 6 , the honeycomb structure 4 further includes a trapping layer 14 for trapping particulate matter (hereinafter also referred to as "PM") in exhaust gas on the inner surface side of the partition walls 1 surrounding the inlet cells 2 a. The trapping layer 14 is a porous layer in which a plurality of non-oxide particles 15 are bonded together via oxides 16. In the trapping layer 14, the thickness T of the oxides 16 bonding adjacent non-oxide particles 15 together is 0.077 μm or more. Furthermore, the trapping layer 14 satisfies the relationship R≦1.0609e^(4.7057×T), where R (μm) is the average particle size of the non-oxide particles constituting the trapping layer 14 and T (μm) is the thickness of the oxides 16. Hereinafter, the relational expression "R≦1.0609e^(4.7057×T)" may be referred to as "relational expression (1)." The left side of relational expression (1) represents the average particle size R (μm) of the non-oxide particles. Meanwhile, on the right side of relational expression (1), e represents Napier's constant, which is the base of natural logarithms. The right side of relational expression (1) represents the value obtained by multiplying 1.0609 by Napier's constant (e), which is exponent of "the value obtained by multiplying the thickness T (μm) of the oxide 16 by 4.7057." Here, FIG. 5 is a cross-sectional view schematically showing a cross section of the partition wall. In FIG. 5, reference numeral 7 denotes a pore formed in the partition wall 1. FIG. 6 is an enlarged cross-sectional view of the trapping layer in the range indicated by reference numeral P in FIG. 5.
[0021] Because the trapping layer 14 is a porous layer composed of the non-oxide particles 15 and the oxide 16 as described above, the trapping layer 14 is less likely to break even when subjected to stress such as vibration or thermal shock, and peeling of the trapping layer 14 from the partition wall 1 can be effectively suppressed. In particular, if the thickness T of the oxide 16 is less than 0.077 μm, the bonding portions bonding the non-oxide particles 15 become thin, making the bonds between the non-oxide particles 15 more likely to be broken. Even if the thickness T of the oxide 16 is 0.077 μm or more, if the above relational expression (1) is not satisfied, the bonding portions bonding the non-oxide particles 15 become thin, making the bonds between the non-oxide particles 15 more likely to be broken. For example, if the average particle size R (μm) of the non-oxide particles is small, the lower limit of the allowable thickness T μm of the oxide 16 also becomes small. Furthermore, as the average particle size R (μm) of the non-oxide particles increases, the lower limit of the allowable thickness T μm of the oxide 16 also increases.
[0022] The thickness T of the oxide 16 that bonds adjacent non-oxide particles 15 together is 0.077 μm or more, and is configured to satisfy the above-mentioned relational expression (1). Although not particularly limited, for example, when the average particle size R of the non-oxide particles is approximately 2.2 to 3.0 μm, the thickness of the oxide 16 is preferably 0.155 to 0.230 μm, and more preferably 0.155 to 0.167 μm. For example, if the thickness of the oxide 16 becomes extremely thick, cracks or the like may occur in the layer made of the oxide 16 that bonds the non-oxide particles 15 together (hereinafter also referred to as the "oxide layer"), making the bonds (bonds) between the non-oxide particles 15 more likely to break. For this reason, although not particularly limited, the upper limit of the thickness of the oxide 16 can be, for example, 0.230 μm.
[0023] There are no particular restrictions on the average particle size R (μm) of the non-oxide particles 15 that make up the trapping layer 14. For example, the average particle size R (μm) of the non-oxide particles 15 is preferably 0.4 to 2.4 μm, and more preferably 0.9 to 2.4 μm. The average particle size R (μm) of the non-oxide particles 15 can be determined by the following method.
[0024] First, a part of the partition walls 1 and the trapping layer 14 is cut out as a test piece from the honeycomb structure 4 constituting the honeycomb filter 100 as shown in Figures 1 to 3. The test piece is cut out from the central cross section in the extension direction of the cells 2 of the honeycomb filter 100 (i.e., the flow path direction) to the outflow end face 12 (however, excluding the portion where the plugging portion 5 on the outflow end face 12 side is arranged).
[0025] Next, the cut-out test piece is cut in a direction perpendicular to the extension direction of the cell 2, and the cut surface is polished. The polishing of the cut surface is performed by mechanical polishing.
[0026] Next, the polished cut surface is imaged using a scanning electron microscope (hereinafter also referred to as "SEM") to obtain an SEM image. "SEM" is an abbreviation for "Scanning Electron Microscope." The imaging conditions are: magnification: 200x, file format: TIF, width: 1280 pixels, height: 960 pixels. SEM images are taken for four fields of view. These four fields of view may be taken at four different points on one test piece, for example, or four test pieces may be prepared and imaged for each test piece. The SEM images for four fields of view are also referred to as "four levels" hereinafter.
[0027] Next, of the non-oxide particles 15 constituting the trapping layer 14 shown in the SEM image, only the non-oxide particles 15 present on the partition walls 1, which are the substrate, are subjected to binarization analysis. That is, the non-oxide particles 15 present inside the pores of the partition walls 1 and the non-oxide particles 15 present across the portion where the partition walls 1 are present are not subjected to binarization analysis. For example, if the partition walls 1 shown in the SEM image are positioned at the bottom of the image, a line is virtually drawn at the boundary corresponding to the surface of the partition walls 1, and only the non-oxide particles 15 present above the line are subjected to binarization analysis. This enables more accurate calculation of the average particle size R (μm) of the non-oxide particles 15. The binarization process is performed using image analysis software "Winroof 2018 (Mitani Corporation) (product name)" manufactured by Mitani Corporation. "Circle equivalent diameter" is selected as the binarization analysis item, and the average particle size R (μm) of the non-oxide particles 15 is calculated.
[0028] The thickness T (μm) of the oxide 16 constituting the trapping layer 14 can be measured as follows. First, a part of the partition walls 1 and the trapping layer 14 is cut out as a test piece from the honeycomb structure 4 constituting the honeycomb filter 100 as shown in Figures 1 to 3. The test piece is cut out from the central cross section in the extension direction of the cells 2 of the honeycomb filter 100 (i.e., the flow path direction) to the outflow end face 12 (however, excluding the area where the plugging portion 5 on the outflow end face 12 side is disposed).
[0029] Next, the cut-out test piece is cut in a direction perpendicular to the extension direction of the cell 2, and the cut surface is polished. The polishing of the cut surface is carried out by mechanical polishing and then ion polishing.
[0030] Next, the polished cut surface is imaged using a field emission scanning electron microscope (hereinafter also referred to as "FE-SEM") to obtain an SEM image at a magnification of 6000x. "FE-SEM" is an abbreviation for "Field Emission Scanning Electron Microscope." The imaging condition is an acceleration voltage of 1.5 kV. SEM images are taken for four fields of view. These four fields of view may be taken at four different points on one test piece, for example, or four test pieces may be prepared and images may be taken for each test piece. The SEM images for four fields of view are hereinafter also referred to as "four levels."
[0031] Next, the constituent components of the trapping layer 14 shown in the SEM image are qualitatively analyzed by EDS analysis to confirm whether the constituent components are oxides or non-oxides.
[0032] Next, image analysis is performed on the trapping layer 14 in the obtained SEM image. In the image analysis, the particles (non-oxide particles 15) with the largest cross-sectional area among the particles constituting the trapping layer 14 in the SEM image are selected as the particles to be measured. Then, the thickness T of the oxide 16 that connects the non-oxide particles 15 is measured at five points on the periphery of the particle to be measured. nThe five measurement points on the periphery of the particle to be measured are determined so as to be evenly spaced along the periphery. The boundary between the surface of the non-oxide particle 15 and the oxide 16 is identified by a white area near the periphery of the particle to be measured in the SEM image. The thickness is measured by measuring the distance between two points on the periphery of the particle to be measured and the boundary. Image analysis is performed using "Image J (product name)" from the National Institutes of Health (NIH). The white area at the boundary between the surface of the non-oxide particle 15 and the oxide 16 is presumably due to the effects of charge-up (electron beam charging). In other words, the SEM image used for image analysis is a secondary electron image, and is affected by charge-up (electron beam charging). Charge-up refers to the phenomenon in which the insulator becomes charged when measuring a sample containing an insulator, resulting in inaccurate results. The difference in conductivity between the non-oxide particle 15 and the oxide 16 creates a slight insulating state, which causes the particle to become charged, resulting in a white area due to charge-up. Since the non-oxide particles 15 and the oxide particles 16 basically have different electrical conductivities, it is possible to distinguish the boundary between them by the density of the image.
[0033] In each level of image analysis, the thickness T of the oxide 16 at seven points on each of the three measurement target particles n Then, of the seven measured points, the maximum and minimum values are excluded from each of the five measured points, and these five points are taken as the measured values for the three particles to be measured. The average value of the five measured points, a total of 15 points, is then calculated. The average values of the four levels are then further averaged to calculate the thickness T of the oxide 16 as the final measured value. Therefore, the thickness T (μm) of the oxide 16 as the final measured value is calculated by multiplying the thickness T of the oxide 16 at a total of 60 points. n The average value of
[0034] The oxide 16 that constitutes the trapping layer 14 constitutes a bonding portion that bonds the non-oxide particles 15 together. The oxide 16 may be any oxide that bonds the non-oxide particles 15 that serve as aggregates in the trapping layer 14 to one another. However, it is preferable that the oxide 16 be disposed so as to cover the surfaces of the non-oxide particles 15. This configuration can further strengthen the bonds between the non-oxide particles 15, making the trapping layer 14 more resistant to destruction and extremely effectively suppressing peeling of the trapping layer 14 from the partition walls 1.
[0035] Although there are no particular limitations on the type of oxide 16 that bonds the non-oxide particles 15, it is preferable that the oxide has a melting point of 1200° C. or higher, and examples thereof include silicon oxide, cerium oxide, titanium oxide, and zirconium oxide. In the honeycomb filter 100 of this embodiment, it is preferable that the oxide 16 is silicon oxide.
[0036] The particles constituting the trapping layer 14 may be particles made of a non-oxide (non-oxide particles 15). Examples of components constituting the non-oxide particles 15 include silicon carbide, cerium, titanium, and zirconium. In the honeycomb filter 100 of this embodiment, the non-oxide particles 15 are preferably silicon carbide particles. By using silicon carbide particles as the non-oxide particles 15, the non-oxide particles 15 can be sintered together, and then the sintered non-oxide particles 15 can be heat-treated under predetermined conditions in an oxidizing atmosphere to easily form oxides 16 that serve as bonding portions between the non-oxide particles 15. In other words, the sintered portions of the non-oxide particles 15 are oxidized, and the sintered portions become silicon oxide (SiO 2 ) and it is possible to easily produce trapping layer 14 consisting of a porous layer in which a plurality of non-oxide particles 15 are bonded via oxide 16. In addition to silicon carbide, with respect to cerium, titanium, and zirconium, the sintered portions of non-oxide particles 15 are also oxidized, and the sintered portions become oxides of the respective components.
[0037] The trapping layer 14 is preferably disposed only on the inner surfaces of the partition walls 1 surrounding the inlet cells 2 a. If the trapping layer 14 is disposed on any surface other than the inner surfaces of the partition walls 1 surrounding the inlet cells 2 a, the pressure loss of the honeycomb filter 100 may increase.
[0038] The average pore diameter of the trapping layer 14 is preferably smaller than the average pore diameter of the partition walls 1. With this configuration, the trapping layer 14 disposed on the inner surface side of the partition walls 1 surrounding the inlet cells 2a can effectively trap PM contained in the exhaust gas.
[0039] The average pore size of the trapping layer 14 is preferably 2 to 9 μm, more preferably 2 to 7 μm, and particularly preferably 3 to 5 μm. There are no particular restrictions on the average particle size R (μm) of the non-oxide particles 15 that make up the trapping layer 14. For example, the average particle size R (μm) of the non-oxide particles 15 is preferably 2.4 μm or less. By setting the average particle size R (μm) of the non-oxide particles 15 to 2.4 μm or less, the bonds between the non-oxide particles 15 can be strengthened, the trapping layer 14 becomes more resistant to fracture, and peeling of the trapping layer 14 from the partition walls 1 can be extremely effectively suppressed.
[0040] The porosity of the trapping layer 14 is preferably 55 to 90%, more preferably 55 to 85%, and particularly preferably 60 to 85%. If the porosity of the trapping layer 14 is less than 55%, the pressure loss may increase. On the other hand, if the porosity of the trapping layer 14 exceeds 90%, the trapping efficiency may deteriorate.
[0041] The porosity and average pore diameter of the trapping layer 14 can be measured by the following method. First, a cross-section of the trapping layer 14 is observed using a scanning electron microscope, and an SEM image of the cross-section is obtained. The SEM image is observed at 200x magnification. Next, the obtained SEM image is analyzed to binarize the solid portion of the trapping layer 14 and the void portion in the trapping layer 14. The percentage of the ratio of the void portion in the trapping layer 14 to the total area of the solid portion and void portion of the trapping layer 14 is then calculated, and this value is used as the porosity of the trapping layer 14. Separately, the voids between each particle size in the SEM image are binarized, and their sizes are directly measured using a scale. The pore diameter in the trapping layer 14 is calculated from the measured value. The average value of the calculated pore diameters is used as the average pore diameter of the trapping layer 14.
[0042] The thickness of the trapping layer 14 is preferably 10 to 60 μm, more preferably 20 to 50 μm, and particularly preferably 20 to 40 μm. If the thickness of the trapping layer 14 is less than 10 μm, the improvement in trapping efficiency may be small, which is undesirable. On the other hand, if the thickness of the trapping layer 14 exceeds 60 μm, the improvement in trapping efficiency may remain high and the pressure loss may increase, which is undesirable.
[0043] The thickness of the trapping layer 14 can be measured by the following method. First, six intersections are determined from a cross section of the honeycomb filter 100 that passes through the central axis of the cell 2 in the extension direction and is parallel to the partition walls 1. The six intersections are the intersections of three lines that divide the cross section into four equal parts in the extension direction of the cells 2 and two lines that divide the cross section into three equal parts in a direction perpendicular to the extension direction of the cells 2. Then, test pieces including an area of 20 mm (vertical) × 20 mm (horizontal) are cut out parallel to the cross section, centered on each intersection. The thickness of the test piece (i.e., the depth parallel to the cross section) can be determined arbitrarily. Any pair of adjacent inlet and outlet cells 2a and 2b is selected from the test piece, and the average surface height of each cell 2 (specifically, the surface height of each cell 2 in the direction perpendicular to the partition walls 1) is measured using a 3D shape measuring device within a range of approximately 8 mm in the extension direction of the cells 2. Next, the difference in surface height between the inflow cell 2 a and the outflow cell 2 b is calculated, and this is taken as the thickness of the trapping layer 14 .
[0044] The average pore diameter of the partition walls 1 is preferably 7 to 19 μm, more preferably 7 to 12 μm, and particularly preferably 7 to 9 μm. The average pore diameter of the partition walls 1 is a value measured by mercury intrusion porosimetry. The average pore diameter of the partition walls 1 can be measured using, for example, an Autopore 9500 (product name) manufactured by Micromeritics. If the average pore diameter of the partition walls 1 is less than 7 μm, the permeation resistance of the partition walls 1 increases, which is undesirable because the pressure loss may increase. If the average pore diameter of the partition walls 1 exceeds 19 μm, it is undesirable from the viewpoint of formability during membrane formation of the trapping layer 14.
[0045] The porosity of the partition walls 1 of the honeycomb structure 4 is preferably 48 to 65%, more preferably 55 to 60%, and particularly preferably 55 to 59%. The porosity of the partition walls 1 is a value measured by mercury porosimetry. The porosity of the partition walls 1 can be measured using, for example, an Autopore 9500 (trade name) manufactured by Micromeritics. If the porosity of the partition walls 1 is less than 48%, the permeation resistance of the partition walls 1 increases, which is undesirable because the pressure loss increases. If the porosity of the partition walls 1 exceeds 65%, it is undesirable because the strength may decrease significantly.
[0046] In the honeycomb structure 4, the thickness of the partition walls 1 is preferably 0.152 to 0.305 mm, more preferably 0.190 to 0.267 mm, and particularly preferably 0.190 to 0.241 mm. The thickness of the partition walls 1 can be measured using, for example, a profile projector. If the thickness of the partition walls 1 is less than 0.152 mm, sufficient strength may not be obtained. On the other hand, if the thickness of the partition walls 1 exceeds 0.305 mm, pressure loss may increase when a trapping layer 14 is disposed on the surface of the partition walls 1.
[0047] The shape of the cells 2 formed in the honeycomb structure 4 is not particularly limited. For example, examples of the shape of the cells 2 in a cross section perpendicular to the extension direction of the cells 2 include polygonal, circular, and elliptical shapes. Examples of polygonal shapes include triangular, rectangular, pentagonal, hexagonal, and octagonal shapes. The shape of the cells 2 is preferably triangular, rectangular, pentagonal, hexagonal, or octagonal. All the cells 2 may have the same shape or different shapes. For example, although not shown in the drawings, a mixture of rectangular and octagonal cells may be used. All the cells 2 may have the same size or different sizes. For example, although not shown in the drawings, among a plurality of cells, some cells may be larger in size and the other cells may be smaller in size. In the present invention, the cell 2 refers to a space surrounded by the partition walls 1.
[0048] The cell density of the cells 2 partitioned and formed by the partition walls 1 is 31 to 62 cells / cm 2 is preferably 31 to 55 particles / cm 2 With this configuration, the filter can be suitably used as a filter for capturing PM in exhaust gas emitted from an engine of an automobile or the like.
[0049] The peripheral wall 3 of the honeycomb structure 4 may be configured integrally with the partition walls 1, or may be an peripheral coating layer formed by applying an peripheral coating material so as to surround the partition walls 1. Although not shown in the drawings, the peripheral coating layer can be provided on the outer periphery of the partition walls during production after the partition walls and the peripheral wall are integrally formed and the formed peripheral wall is removed by a known method such as grinding.
[0050] There is no particular limitation on the shape of the honeycomb structure 4. The honeycomb structure 4 may have an inflow end face 11 and an outflow end face 12 that are cylindrical, elliptical, polygonal, or the like.
[0051] There are no particular limitations on the size of the honeycomb structure 4, for example, the length in the direction in which the cells 2 of the honeycomb structure 4 extend (hereinafter also referred to as the "total length") and the size of the cross section of the honeycomb structure 4 perpendicular to the direction in which the cells 2 extend (hereinafter also referred to as the "cross-sectional area"). Each size may be selected appropriately so that optimal purification performance is obtained when the honeycomb filter 100 is used. The total length of the honeycomb structure 4 is preferably 90 to 160 mm, and more preferably 120 to 140 mm. The cross-sectional area of the honeycomb structure 4 is 8000 to 16000 mm. 2 It is preferable that the thickness is 10,000 to 14,000 mm 2 It is more preferable that:
[0052] The material of the partition walls 1 preferably contains at least one selected from the group consisting of cordierite, silicon carbide, silicon-silicon carbide composite materials, mullite, alumina, aluminum titanate, silicon nitride, and silicon carbide-cordierite composite materials. The material constituting the partition walls 1 is preferably a material containing 30 mass% or more of the materials listed in the above group, more preferably a material containing 40 mass% or more, and particularly preferably a material containing 50 mass% or more. In the honeycomb filter 100 of the present embodiment, the material constituting the partition walls 1 is particularly preferably cordierite.
[0053] (2) Method for Manufacturing Honeycomb Filter: The method for manufacturing the honeycomb filter of the present invention is not particularly limited, and examples thereof include the following methods.
[0054] First, a plastic clay for producing the partition walls of the honeycomb structure is prepared. The clay for producing the partition walls of the honeycomb structure can be prepared by appropriately adding additives such as binders, pore-forming materials, and water to the raw material powder for producing the above-mentioned suitable material for the partition walls. Examples of the raw material powder that can be used include powders of alumina, talc, kaolin, and silica. Examples of the binder include methylcellulose and hydroxypropyl methylcellulose. Examples of the additive include surfactants.
[0055] The thus obtained clay is then extruded to produce a columnar honeycomb formed body having partition walls that define a plurality of cells and an outer peripheral wall that surrounds the partition walls. The obtained honeycomb formed body is then dried, for example, by microwaves and hot air.
[0056] Next, plugging portions are formed on the dried honeycomb formed body. The method for forming the plugging portions can be performed in accordance with a conventionally known method for manufacturing a honeycomb filter. For example, first, a mask is applied to the inlet end face of the honeycomb formed body so that the inlet cells are covered. Then, plugging slurry is applied to the end face of the honeycomb formed body where the mask is applied, and the plugging slurry is filled into the openings of the outlet cells where the mask is not applied. Then, the plugging slurry is filled into the openings of the inlet cells on the outlet end face of the honeycomb formed body in the same manner as above. Then, the honeycomb formed body with the plugging portions formed thereon is further dried in a hot air dryer.
[0057] Next, the honeycomb formed body with the plugged portions formed therein is fired to produce a honeycomb filter precursor before the trapping layer is disposed. Note that the firing temperature and firing atmosphere when firing the honeycomb formed body differ depending on the raw materials used to produce the honeycomb formed body, and a person skilled in the art can select the firing temperature and firing atmosphere that are optimal for the selected materials.
[0058] Next, non-oxide particles for forming the trapping layer are prepared. The prepared non-oxide particles are then flowed into the cells of the honeycomb filter precursor, and the non-oxide particles are adhered to the surfaces of the partition walls of the honeycomb filter precursor. The method for flowing the non-oxide particles into the cells of the honeycomb filter precursor is not particularly limited, but examples include a method in which the non-oxide particles are dispersed in a gas to form an aerosol, and the aerosol is then flowed into the cells. A suitable example of the non-oxide particles is silicon carbide particles. There are no particular limitations on the average particle size of the silicon carbide particles, but it is preferable that the average particle size be 0.4 to 2.4 μm, for example.
[0059] As described above, non-oxide particles are attached to the inner surface side of the partition walls surrounding the inlet cells of the honeycomb filter precursor to form a film, and then the formed non-oxide particles are oxidized (heat treated) at 600°C or higher in an air atmosphere to bond the non-oxide particles together. By configuring in this way, the sites bonding the non-oxide particles together become oxides, and a trapping layer made of a porous layer in which a plurality of non-oxide particles are bonded via oxides is formed on the inner surface side of the partition walls surrounding the inlet cells of the honeycomb filter precursor. For example, when silicon carbide particles are used to form a film, the sites bonding the silicon carbide particles together become silicon oxide (SiO 2), which allows for the easy production of a trapping layer consisting of a porous layer in which multiple non-oxide particles are bonded via an oxide. There are no particular limitations on the temperature and time for oxidizing (heat treating) the formed non-oxide particles. However, it is preferable to continue oxidation until the thickness of the region (silicon oxide) bonding the silicon carbide particles together reaches 0.077 μm or more and the above-mentioned relational expression (1) is satisfied. For example, the oxidation temperature is preferably 800 to 1400°C, and the oxidation time is preferably 1 to 4 hours. The oxidation temperature and oxidation time are heat treatment conditions that affect the thickness of the oxide bonding the non-oxide particles together. However, just because either the oxidation temperature or the oxidation time satisfies the above-mentioned numerical range does not necessarily mean that the oxide thickness will be a certain value or greater. It is preferable to appropriately select heat treatment conditions that result in a certain value or greater of oxide thickness while adjusting the oxidation temperature and oxidation time within the above-mentioned numerical range. Furthermore, the amount of oxide produced can also be determined from the mass increase before and after oxidation (heat treatment). For example, when silicon carbide particles are used as the non-oxide particles, if the mass increase after heat treatment is 20% or more relative to the mass of the raw material particles used, the thickness of the silicon oxide, which is the bonding site, can be 0.077 μm or more and satisfy the above-mentioned relational expression (1). For example, although not particularly limited, if the average particle size R of the non-oxide particles is approximately 2.2 to 3.0 μm, the thickness of the silicon oxide can be 0.155 μm or more. The formed non-oxide particles can be oxidized, for example, by charging the honeycomb filter precursor into an electric furnace or by heating the non-oxide particles attached to the inner surface side of the partition walls with a gas burner. In this manner, the honeycomb filter of the present invention can be manufactured.
[0060] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0061] Example 1 First, alumina, talc, kaolin, and silica raw materials for producing partition walls of a honeycomb structure were prepared. 2 parts by mass of a dispersion medium and 7 parts by mass of an organic binder were added to the prepared alumina, talc, kaolin, and silica raw materials, respectively, and the mixture was mixed and kneaded to prepare a clay. Water was used as the dispersion medium. Methyl cellulose was used as the organic binder. A surfactant was used as the dispersant.
[0062] Next, the clay was extruded using a die for producing a honeycomb formed body to obtain a honeycomb formed body having an overall cylindrical shape. The shape of the cells of the honeycomb formed body was rectangular.
[0063] Next, the honeycomb formed body was dried in a microwave dryer and further completely dried in a hot air dryer, after which both end faces of the honeycomb formed body were cut and adjusted to a predetermined size.
[0064] Next, plugging portions were formed on the dried honeycomb formed body. Specifically, first, a mask was applied to the inlet end face of the honeycomb formed body so that the inlet cells were covered. Then, plugging slurry was applied to the end face of the masked honeycomb formed body, and the plugging slurry was filled into the openings of the outlet cells that were not masked. Thereafter, the plugging slurry was filled into the openings of the inlet cells on the outlet end face of the honeycomb formed body in the same manner as above. Thereafter, the honeycomb formed body with the plugging portions formed thereon was further dried in a hot air dryer.
[0065] Next, the dried honeycomb formed body was degreased and fired to produce a honeycomb filter precursor before the trapping layer was disposed thereon.
[0066] Next, a trapping layer was formed on the inner surface side of the partition walls surrounding the inlet cells of the honeycomb filter precursor by the following method. Specifically, first, silicon carbide particles having an average particle diameter (median diameter) of 2.4 μm were prepared. Next, the prepared silicon carbide particles were dispersed in a gas to form an aerosol, and the aerosol was allowed to flow into the inlet cells. In this way, a film of silicon carbide particles was formed on the inner surface side of the partition walls surrounding the inlet cells. Specific film formation conditions for the silicon carbide particles are as follows. Aerosol generator: RBG2000 manufactured by PALAS Rotating body: rotating brush Non-oxide particles contained in container: silicon carbide particles (SiC particles) Median diameter (D50): 2.4 μm D10: 1.1 μm D90: 4.5 μm (based on volume-based cumulative particle size distribution measured by laser diffraction / scattering method) Mass of sprayed non-oxide particles: 6.0 g Medium gas: compressed dry air (dew point 10°C or less) Ambient gas: air Average flow velocity of aerosol flowing into honeycomb filter precursor: 3 m / s Laser diffraction particle size distribution measuring device: InsitecSpray manufactured by MALVERN Operating time: 20 seconds Inner diameter of aerosol generator nozzle: 8 mm diameter Distance from the tip of the aerosol generator nozzle to the inlet end face of the honeycomb filter precursor: 1000 mm Aerosol spray velocity: 20 m / s
[0067] Next, the honeycomb filter precursor coated with silicon carbide particles was placed in an electric furnace and subjected to heat treatment at 1200°C in an air atmosphere. The heat treatment was maintained at 1200°C for 2.2 hours. This heat treatment formed a trapping layer on the inner surface of the partition walls surrounding the inlet cells, in which silicon carbide particles were bonded together by silicon oxide. The above-described heat treatment oxidized a portion of the particles (silicon carbide particles) used as the raw material for the trapping layer, resulting in a 20% increase in mass after the heat treatment relative to the mass of the raw material used. The 20% mass increase due to the heat treatment was due to oxidation progressing from the surface side of the silicon carbide particles, resulting in the surface side of the silicon carbide particles and the sites bonding the silicon carbide particles becoming oxide (silicon oxide). The thickness of the oxide at the sites bonding the silicon carbide particles was measured using the method described above, and the oxide thickness was 0.155 μm. The results are shown in Table 1. The honeycomb filter produced as described above was used as the honeycomb filter of Example 1.
[0068] The honeycomb filter of Example 1 had a cylindrical shape with circular inlet and outlet end faces. The length of the honeycomb filter in the cell extension direction was 120 mm. The diameter of the end face of the honeycomb filter was 132 mm. The partition walls of the honeycomb structure had a porosity of 60%. The average pore diameter of the partition walls was 12 μm. The porosity and average pore diameter of the partition walls were measured using an Autopore 9500 (trade name) manufactured by Micromeritics. The results are shown in Table 1. The honeycomb structure constituting the honeycomb filter had a partition wall thickness of 0.216 mm and a cell density of 31 cells / cm. 2 It was.
[0069]
[0070] The honeycomb filter of Example 1 was subjected to a peeling test of the trapping layer by the following method. The results are shown in Table 1.
[0071] [Peeling Test (Peeling Test of Trapping Layer)] First, the honeycomb filter 100 to be tested was mounted on the sample mounting section 41 of a vibration tester 20 as shown in FIG. 7, and a peeling test of the trapping layer was performed. FIG. 7 is a schematic plan view illustrating the configuration of a vibration tester for performing a peeling test of the trapping layer. As shown in FIG. 7, the vibration tester 20 includes a burner section 21 and a vibration section 31. The burner section 21 has a combustion chamber 24 in which a main burner 22 and a pilot burner 23 are disposed. The main burner 22 and the pilot burner 23 are burners that use liquefied petroleum gas (LPG) as fuel, and pilot air is supplied to the pilot burner 23 in addition to the fuel. The combustion chamber 24 is supplied with combustion air for burning the fuel and cooling air for cooling the honeycomb filter 100 when combustion is stopped. The vibration unit 31 is disposed below the sample mounting unit 41 that mounts the honeycomb filter 100, and applies up and down vibrations to the sample mounting unit 41. The sample mounting unit 41 is configured so that air heated by the burner unit 21 flows while vibrations from the vibration unit 31 are applied to the honeycomb filter 100 mounted therein. In the peeling test, a cycle test was performed in which heated air heated by the burner and cooling air for cooling were alternately and repeatedly flowed under the following conditions while the vibration unit 31 applied vibrations to the honeycomb filter 100 at a vibration frequency of 150 Hz and a gravitational acceleration of 40 g. The heated air flowed into the honeycomb filter 100 at an inlet temperature of 900°C and a flow rate of 2.0 Nm 3 / min. After flowing this heated air for 5 minutes, the combustion of the main burner 22 and the pilot burner 23 was stopped, and cooled air was flowed for 5 minutes. A peeling test was conducted by alternately flowing heated air and cooled air 75 times in this manner. After the peeling test, the honeycomb filter 100 was removed from the sample mounting section 41, and the mass (mass loss) of the honeycomb filter 100 before and after the test was measured. A test was considered to pass if the mass loss after the test was less than 3% of the trapping layer mass and the loss in filtering efficiency after the test was less than the measurement variance (2σ) calculated from the results of 30 or more repeated measurements of the honeycomb filter before the test under the measurement conditions. Such a pass is indicated as "OK" in Table 1. On the other hand, a test was considered to fail if the mass loss after the test was 3% or more of the trapping layer mass and the loss in filtering efficiency after the test was greater than the measurement variance (2σ) calculated from the results of 30 or more repeated measurements of the honeycomb filter before the test under the measurement conditions. Such failures are marked as "NG" in Table 1.
[0072] (Examples 2 to 13, Comparative Examples 1 to 3) The configuration of the honeycomb structure, and the configuration and manufacturing method of the trapping layer were changed as shown in Tables 1 and 2 to manufacture honeycomb filters of Examples 2 to 13 and Comparative Examples 1 to 3. In Examples 2 to 5 and Comparative Example 3, the heat treatment of the trapping layer was performed by heating a honeycomb filter precursor coated with silicon carbide particles using a gas burner. A trapping layer peeling test was also performed on the honeycomb filters of Examples 2 to 13 and Comparative Examples 1 to 3 using the same method as in Example 1. The results are shown in Tables 1 and 2. Note that Examples 1 to 13 satisfy the previously explained relational expression (1): R≦1.0609e^(4.7057×T). On the other hand, Comparative Examples 1 to 3 do not satisfy the above-mentioned relational expression (1).
[0073]
[0074] (Results) The honeycomb filters of Examples 1 to 13 had oxide thicknesses T of 0.077 μm or more and satisfied the above-mentioned relational expression (1), and no peeling of the trapping layer was confirmed in the trapping layer peeling test, resulting in an OK (pass) result. On the other hand, the honeycomb filters of Comparative Examples 1 to 3 did not satisfy the relational expression (1): R≦1.0609e^(4.7057×T) even though they had oxide thicknesses T of 0.077 μm or more, and peeling of the trapping layer was confirmed in the trapping layer peeling test.
[0075] The honeycomb filter of the present invention can be used as a filter for collecting particulate matter in exhaust gases.
[0076] 1: Partition wall, 2: Cell, 2a: Inlet cell, 2b: Outlet cell, 3: Outer peripheral wall, 4: Honeycomb structure, 5: Plugging portion, 7: Pore, 11: Inlet end face, 12: Outlet end face, 14: Trapping layer, 155: Non-oxide particles, 16: Oxide, 20: Vibration tester, 21: Burner portion, 22: Main burner, 23: Pilot burner, 24: Combustion chamber, 31: Vibration portion, 41: Sample mounting portion, 100: Honeycomb filter.
Claims
1. A honeycomb structure having porous partition walls arranged to surround a plurality of cells which form a fluid flow path extending from an inflow end face to an outflow end face, and plugging portions arranged to plug either one of the inflow end face side or the outflow end face side of the cells, wherein the plugging portions are arranged at the ends on the outflow end face side and the cells which are open on the inflow end face side are defined as inflow cells, and the plugging portions are arranged at the ends on the inflow end face side and the cells which are open on the outflow end face side are defined as outflow cells, and the honeycomb structure further has a collection layer for collecting particulate matter in exhaust gas on the inner surface side of the partition walls which surround the inflow cells, The trapping layer is a porous layer in which a plurality of non-oxide particles are bonded together via an oxide, and the thickness of the oxide bonding adjacent non-oxide particles is 0.077 μm or more. In addition, when the average particle size of the non-oxide particles constituting the trapping layer is R (μm) and the thickness of the oxide is T (μm), the relationship R≦1.0609e^(4.7057×T) is satisfied.
2. The honeycomb filter according to claim 1, wherein the oxide constituting the collection layer is disposed so as to cover the surfaces of the non-oxide particles.
3. A honeycomb filter according to claim 1 or 2, wherein the non-oxide particles are silicon carbide particles.
Citation Information
Patent Citations
Silicon carbide based porous compact and method for manufacturing the same
JP2002356383A
Exhaust gas purification device for internal combustion engine, production method of the same and paint for producing exhaust gas purification device
JP2015199066A
Exhaust gas purification filter, exhaust gas purification apparatus, and using method for exhaust gas purification apparatus
JP2016182536A
Honeycomb structure, honeycomb filter for exhaust gas purification, and exhaust gas purification device
WO2013145245A1
Honeycomb filter, exhaust gas purification device, and exhaust gas purification method
WO2013175552A1