Heat-sealable paper and packaging bag
The heat-seal paper with a water-dispersible resin and specific wetting agents addresses the plastic waste issue by offering enhanced heat-sealing and anti-blocking properties, suitable for various packaging needs, thus providing an eco-friendly alternative to traditional plastic packaging.
Patent Information
- Application Number
- PCT/JP2024/010952
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-03
AI Technical Summary
Current heat-seal packaging solutions, particularly using plastic, contribute significantly to plastic waste and ecosystem damage, necessitating the development of alternative materials with excellent heat-sealing and anti-blocking properties for various industrial and food packaging applications.
A heat-seal paper with a heat-sealing layer containing a water-dispersible resin and a wetting agent, where the resin has a glass transition temperature of 0°C or higher, and the wetting agent is acetylene, acrylic, or silicone-based, applied to a paper base material with a surface roughness of 12.0 μm or more, enhancing heat-sealability and blocking resistance.
The solution provides heat-seal paper with improved heat-sealing properties and anti-blocking capabilities, suitable for diverse packaging applications, including food and household goods, while reducing plastic waste.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002
Abstract
Description
Heat-seal paper and packaging bags
[0001] The present invention relates to heat seal paper and a packaging bag using the same.
[0002] Packages using the heat seal method are widely used for packaging general industrial products as well as for packaging food, medicines, medical equipment, and the like.
[0003] The problem of plastic waste has become more serious in recent years. Of the total amount of plastic produced worldwide, a large amount is produced in the packaging sector, which is the cause of plastic waste. Plastic does not decompose for a long time, and this waste breaks down into microplastics in the natural environment, causing serious damage to the ecosystem. As a countermeasure, it has been proposed to replace plastic with paper.
[0004] For example, Japanese Patent No. 7070785 discloses a heat-sealable paper having at least one heat-sealable layer on at least one side of a paper base material, the heat-sealable layer containing a water-dispersible resin binder and further containing a lubricant, and when the heat-sealable layers are heat-sealed together under conditions of 150°C, 0.2 MPa, and 1 second, the hot tack peel distance is 150 mm or less, the heat-seal peel strength is 2 N / 15 mm or more, and the pulp recovery rate after re-defibration is 85% or more. Furthermore, Japanese Patent Application Laid-Open No. 2022-175023 discloses a heat-sealable paper having at least one heat-sealable layer on at least one side of a paper substrate, the heat-sealable layer containing a pigment having an aspect ratio of 20 or more and a heat-sealable resin, and when the heat-sealable layers are heat-sealed together under conditions of a sealing pressure of 0.2 MPa, a sealing temperature of 140°C, and a sealing time of 1 second, the peel strength is 3 N / 15 mm or more, the Oken air permeability resistance is 2000 seconds or more, and the water repellency on both sides is R6 or more.
[0005] The applications of heat-sealed packaging are expanding, and there is a demand for heat-sealable paper that has excellent blocking resistance during storage and is suitable for a variety of uses.
[0006] An object of the present invention is to provide heat seal paper having excellent heat sealing properties and blocking resistance, and a packaging bag using said heat seal paper.
[0007] The problems of the present invention can be solved by the following configurations <1> to <9>. <1> A heat-sealable paper having a heat-sealable layer on one side of a paper substrate, wherein the heat-sealable layer contains a water-dispersible resin and a wetting agent, the water-dispersible resin contains a water-dispersible resin having a glass transition temperature of 0°C or higher, the content of the wetting agent is 0.04 parts by mass or more and 1.2 parts by mass or less per 100 parts by mass of the water-dispersible resin, and the surface of the heat-sealable paper opposite to the side having the heat-sealable layer has a surface roughness (RzJIS) of 12.0 μm or more. <2> The heat-sealable paper according to <1>, wherein the wetting agent contains at least one selected from the group consisting of an acetylene-based wetting agent, an acrylic-based wetting agent, and a silicone-based wetting agent. <3> The heat-sealable paper according to <1> or <2>, wherein the water-dispersible resin contains a styrene-butadiene-based copolymer. <4> The heat sealable paper according to any one of <1> to <3>, wherein the water-dispersible resin contains a styrene-butadiene copolymer and the wetting agent contains an acetylene-based wetting agent. <5> The heat sealable paper has a basis weight of 50 g / m 2 140g / m or more 2 <6> The heat-sealable paper according to any one of <1> to <4>, wherein the paper substrate is a stretched paper. <7> The heat-sealable paper according to any one of <1> to <5>, wherein the basis weight of the heat-sealable layer is 7 g / m 2 21g / m or more 2 The heat-sealable paper according to any one of <1> to <6>, which is as follows: <8> The heat-sealable paper according to any one of <1> to <7>, which has a heat-seal peel strength of 6.0 N / 15 mm or more when the heat-sealable layers are heat-sealed together under conditions of 160°C, 0.3 MPa, and 0.5 seconds. <9> A packaging bag using the heat-sealable paper according to any one of <1> to <8>.
[0008] Preferred embodiments of the present invention will be described below. In this specification, the range "X to Y" means "X or more and Y or less." When numerical ranges are described in stages, the upper and lower limits of each numerical range can be combined arbitrarily. In this specification, unless otherwise specified, operations and measurements of physical properties are performed at room temperature (20 to 25°C) and a relative humidity of 40 to 50% RH. In addition, "(meth)acrylic" is a generic term that includes both acrylic and methacrylic. In addition, "wetting agent" includes a leveling agent.
[0009] <Heat-seal Paper> The heat-seal paper of this embodiment (hereinafter simply referred to as "heat-seal paper") is a heat-seal paper having a heat-seal layer on one side of a paper substrate, the heat-seal layer containing a water-dispersible resin and a wetting agent, the water-dispersible resin containing a water-dispersible resin with a glass transition temperature of 0°C or higher, the content of the wetting agent being 0.04 parts by mass or more and 1.2 parts by mass or less per 100 parts by mass of the water-dispersible resin, and the surface roughness (RzJIS) of the side of the heat-seal paper opposite to the side having the heat-seal layer is 12.0 μm or more. The heat-seal paper of this embodiment has excellent heat-sealing properties and blocking resistance. Hereinafter, the side of the paper substrate having the heat-seal layer may be simply referred to as the "coated side." For convenience, the side of the paper substrate or heat-seal paper opposite to the side having the heat-seal layer may be referred to as the "uncoated side." However, this does not exclude forms in which a coating layer is present on the side of the paper substrate or heat-seal paper opposite to the side having the heat-seal layer. When no layer is formed by coating or the like on the surface of the paper substrate opposite to the surface having the heat seal layer, the surface of the paper substrate opposite to the surface having the heat seal layer is the uncoated surface.
[0010] Forming a heat-seal layer containing a water-dispersible resin with a glass transition temperature of 0°C or higher and a wetting agent improves the wettability of the paper substrate and the heat-seal layer coating solution during the formation of the heat-seal layer, allowing the water-dispersible resin to uniformly penetrate the paper substrate, enhancing adhesion between the heat-seal layer and the paper substrate, thereby enabling excellent heat-sealability to be achieved by heating, etc. By controlling the amount of wetting agent per 100 parts by mass of water-dispersible resin to a range of 0.04 to 1.2 parts by mass and increasing the surface roughness (RzJIS) of the uncoated surface to 12.0 μm or more, it is believed that the desired heat-sealability can be achieved by heating, etc., and blocking between the heat-seal layer and the uncoated surface can be suppressed during storage (especially when the heat-seal layer is coated, wound around a roll, and stored in a pressure-bonded state). The effects of the present invention are not limited by the above mechanism.
[0011] [Paper base material] (Raw material pulp) The pulp constituting the paper base material is not particularly limited, and known pulps can be used. Specific examples include unbleached pulps such as hardwood unbleached kraft pulp (LUKP) and softwood unbleached kraft pulp (NUKP); chemical pulps such as hardwood bleached kraft pulp (LBKP) and softwood bleached kraft pulp (NBKP); mechanical pulps such as groundwood pulp (GP), pressure groundwood pulp (PGW), refiner mechanical pulp (RMP), thermomechanical pulp (TMP), chemithermomechanical pulp (CTMP), chemi-mechanical pulp (CMP), and chemi-ground pulp (CGP); recycled paper pulp; non-wood fiber pulps such as kenaf, bagasse, bamboo, and cotton; and synthetic pulp. These pulps may be used alone or in combination of two or more. Among these, from the viewpoint of obtaining heat seal paper with the desired surface roughness (RzJIS) on the uncoated side, at least one selected from the group consisting of hardwood unbleached kraft pulp (LUKP), softwood unbleached kraft pulp (NUKP), hardwood bleached kraft pulp (LBKP), and softwood bleached kraft pulp (NBKP) is preferred, at least one selected from the group consisting of hardwood unbleached kraft pulp (LUKP) and softwood unbleached kraft pulp (NUKP) is more preferred, and softwood unbleached kraft pulp (NUKP) is even more preferred.
[0012] The pulp constituting the paper base material used in the heat-seal paper of this embodiment is preferably primarily softwood pulp, and more preferably softwood unbleached kraft pulp (NUKP). "The pulp constituting the paper base material is primarily softwood pulp (or softwood unbleached kraft pulp)" means that the content of softwood pulp (or softwood unbleached kraft pulp) in the pulp constituting the paper base material is more than 50% by mass, and the content of softwood pulp (or softwood unbleached kraft pulp) is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 100% by mass. Softwood pulp has a long average fiber length, and using a paper base material using softwood pulp as the raw material pulp is preferred because it allows heat-seal paper to be obtained with the desired surface roughness (RzJIS) on the uncoated side. Furthermore, when softwood unbleached kraft pulp (NUKP) is used as the pulp that constitutes the paper base material, the strength of the pulp fibers themselves is higher than that of softwood bleached kraft pulp (NBKP) or hardwood unbleached kraft pulp (LUKP), and this has the advantage that the strength and elongation of the resulting paper base material are higher.
[0013] The raw material pulp constituting the paper base material is preferably one or more selected from the group consisting of bleached kraft pulp and unbleached kraft pulp, and more preferably unbleached kraft pulp.
[0014] From the viewpoint of obtaining heat-sealable paper with the desired surface roughness (RzJIS) and arithmetic mean roughness (Ra) on the uncoated side, it is preferable to use Clupak paper (stretched paper) that has been subjected to Clupak treatment to shrink the paper web. Stretched paper refers to paper that has an elongation of 5% or more in the machine or cross direction as measured in accordance with JIS P 8113:2006, and examples include Kraft paper Type 5 Nos. 1 and 2 described in JIS P 3401:2000.
[0015] (Basis Weight) The basis weight of the paper substrate is not particularly limited, but is preferably 40 g / m from the following viewpoints: 2 130g / m or more 2 The basis weight of the paper substrate is preferably 40 g / m from the viewpoint of obtaining a heat seal paper with the desired strength. 2More preferably, 50 g / m 2 More preferably, 60 g / m 2 More preferably, 70 g / m 2 From the viewpoint of bag-making processability and economic efficiency, it is preferably 130 g / m 2 or less, more preferably 110 g / m 2 The basis weight of the paper substrate is measured in accordance with JIS P 8124:2011.
[0016] (Thickness) The thickness of the paper substrate is not particularly limited, but is preferably 50 μm or more and 200 μm or less from the following viewpoints. From the viewpoint of obtaining heat-sealable paper of the desired strength, the thickness of the paper substrate is preferably 50 μm or more, more preferably 60 μm or more, even more preferably 80 μm or more, and even more preferably 100 μm or more. From the viewpoint of bag-making processability and economic efficiency, the thickness is preferably 200 μm or less, more preferably 180 μm or less, and even more preferably 160 μm or less. When the thickness of the paper substrate is within the above-mentioned preferred range, the heat-sealable paper of this embodiment is suitable for use in packaging bags. The thickness of the paper substrate is measured in accordance with JIS P 8118:2014.
[0017] (Density) The density of the paper substrate is not particularly limited, but is preferably 0.3 g / cm from the following viewpoints: 3 1.0g / cm or more 3 The density of the paper substrate is preferably 0.3 g / cm or less from the viewpoint of obtaining a heat seal paper with a desired strength. 3 More preferably, 0.5 g / cm 3 From the viewpoint of bag-making processability and economic efficiency, it is preferably 1.0 g / cm 3 or less, more preferably 0.9 g / cm 3 More preferably 0.75 g / cm or less 3 The density of the paper substrate is calculated from the basis weight and thickness of the paper substrate obtained by the above-mentioned measurement method.
[0018] (Stockigt sizing degree) The Stockigt sizing degree of the uncoated surface of the paper substrate is not particularly limited, but is preferably 30 seconds or more and 100 seconds or less from the following viewpoint. From the viewpoint of improving the strength when used as a packaging bag, particularly from the viewpoint of maintaining strength even when contacted with water, the Stockigt sizing degree of the uncoated surface of the paper substrate is preferably 30 seconds or more, more preferably 40 seconds or more, and even more preferably 50 seconds or more. The upper limit is not particularly limited, but from the viewpoint of economy, it is preferably 100 seconds or less, more preferably 90 seconds or less, even more preferably 85 seconds or less, and even more preferably 80 seconds or less. The Stockigt sizing degree of the coated surface of the paper substrate is not particularly limited, but is preferably 30 seconds or more and 100 seconds or less from the following viewpoint. The Stockigt sizing degree of the coated surface of the paper substrate is preferably 100 seconds or less, more preferably 90 seconds or less, even more preferably 85 seconds or less, and even more preferably 80 seconds or less. When the heat seal layer is equal to or less than the upper limit, the heat seal layer spreads appropriately on the paper substrate, forming a uniform heat seal layer and improving the heat seal peel strength. The preferred lower limit and the reason for this are the same as those for the Stoeckigt sizing degree of the uncoated surface. The Stoeckigt sizing degree is measured in accordance with JIS P 8122:2004. The Stoeckigt sizing degree of the paper substrate can be controlled by the type and amount of surface sizing agent used.
[0019] [Heat-seal layer] The heat-seal paper of this embodiment has a heat-seal layer on one side of the paper substrate. The heat-seal layer contains a water-dispersible resin and a wetting agent, and is a layer that melts and adheres when heated, ultrasonically, or the like. The heat-seal paper of this embodiment preferably has a heat-seal layer as the uppermost layer on one side of the paper substrate. The heat-seal paper of this embodiment may have, for example, a clay coat layer, a gas barrier layer, and / or a water vapor barrier layer between the paper substrate and the heat-seal layer, but preferably has a heat-seal layer directly on one side of the paper substrate.
[0020] (Water-dispersible resin) A water-dispersible resin is a resin binder that is not water-soluble (specifically, has a solubility in water at 25°C of 10 g / L or less), but is finely dispersed in water like an emulsion or suspension.
[0021] The water-dispersible resin includes a water-dispersible resin having a glass transition temperature of 0° C. or higher. The water-dispersible resin having a glass transition temperature of 0° C. or higher is not particularly limited as long as it exhibits the effects of the present invention, except that the glass transition temperature is 0° C. or higher. Examples of the water-dispersible resin include polyolefin resins (polypropylene, etc.), vinyl chloride resins, styrene resins, styrene-butadiene copolymers, styrene-unsaturated carboxylic acid copolymers (for example, styrene-(meth)acrylic acid copolymers), acrylic resins, acrylonitrile-styrene copolymers, acrylonitrile-butadiene copolymers, ABS resins, AAS resins, AES resins, vinylidene chloride resins, polyurethanes, Examples of suitable resins include styrene-based resins, poly(4-methylpentene-1) resins, poly(butene-1) resins, vinylidene fluoride-based resins, vinyl fluoride-based resins, fluorine-based resins, polycarbonate-based resins, polyamide-based resins, acetal-based resins, polyphenylene oxide-based resins, polyester-based resins (polyethylene terephthalate, polybutylene terephthalate, etc.), polyphenylene sulfide-based resins, polyimide-based resins, polysulfone-based resins, polyethersulfone-based resins, polyarylate-based resins, olefin / unsaturated carboxylic acid-based copolymers, and modified products thereof. These may be used alone or in combination of two or more. Among these, styrene-butadiene-based copolymers are more preferred from the viewpoints of the heat sealability, blocking resistance, cost, etc. of the heat seal paper.
[0022] The styrene-butadiene copolymer may be either a synthetic product or a commercially available product. Examples of commercially available products include Nipol Latex LX407G51, LX407S10, LX407S12, LX410, LX415M, LX416, LX430, LX433C, and 2507H manufactured by Nippon Zeon Co., Ltd., Nalustar SR-102, SR-103, SR-115, and SR-153 manufactured by Nippon A&L Inc., and Styrene Butadiene Latex 0602 and 0597C manufactured by JSR Corporation.
[0023] The glass transition temperature of the water-dispersible resin is 0°C or higher from the viewpoint of blocking resistance. The glass transition temperature of the water-dispersible resin is preferably 0°C or higher and 80°C or lower, preferably 3°C or higher, more preferably 6°C or higher, more preferably 70°C or lower, even more preferably 60°C or lower, still more preferably 50°C or lower, even more preferably 40°C or lower, still more preferably 30°C or lower, and even more preferably 20°C or lower. The glass transition temperature of the water-dispersible resin is preferably above the above lower limit from the viewpoint of blocking resistance, and is preferably below the above upper limit from the viewpoint of heat sealability. The glass transition temperature of the water-dispersible resin binder is a value measured by a differential scanning calorimeter (measurement method).
[0024] The content of the water-dispersible resin in the heat-seal layer is preferably 60% by mass or more and 99% by mass or less, more preferably 70% by mass or more, even more preferably 80% by mass or more, and more preferably 98% by mass or less. Within the above range, a heat-sealable paper having high heat-seal strength can be obtained.
[0025] According to one embodiment of the present invention, the content of the styrene-butadiene copolymer in the water-dispersible resin is preferably 85% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and preferably 100% by mass or less.
[0026] The water-dispersible resin may contain a water-dispersible resin having a glass transition temperature of less than 0°C. However, the content of the water-dispersible resin having a glass transition temperature of less than 0°C in the water-dispersible resin is preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 1% by mass or less (lower limit: 0% by mass).
[0027] (Wetting Agent) The heat seal layer contains a wetting agent. Examples of wetting agents include acetylene-based wetting agents, acrylic wetting agents, and silicone-based wetting agents. From the viewpoint of heat sealability and blocking resistance, the wetting agent preferably contains one selected from the group consisting of acetylene-based wetting agents, acrylic wetting agents, and silicone-based wetting agents, and more preferably contains an acetylene-based wetting agent. Furthermore, from the viewpoint of heat sealability and blocking resistance, it is preferable that the water-dispersible resin contains a styrene-butadiene copolymer and that the wetting agent contains an acetylene-based wetting agent.
[0028] The acetylene-based wetting agent is a compound having an acetylene skeleton, and examples thereof include compounds having an acetylene skeleton and a functional group such as a hydroxy group. Among these, acetylene glycol-based wetting agents are preferred. Examples of acetylene glycol-based wetting agents include acetylene glycol and alkylene oxide (e.g., ethylene oxide, propylene oxide) adducts of acetylene glycol, with alkylene oxide adducts of acetylene glycol (alkylene group having 2 to 10 carbon atoms) being preferred, and ethylene oxide adducts of acetylene glycol and propylene oxide adducts of acetylene glycol being more preferred. As the acetylene-based wetting agent, either a synthetic product or a commercially available product may be used, and examples of commercially available products include "Meikasurf S-28" manufactured by Meisei Chemical Industry Co., Ltd. and "Surfynol Series" manufactured by Nissin Chemical Industry Co., Ltd.
[0029] The acrylic wetting agent is a compound having an acryloyl skeleton. Either a synthetic product or a commercially available product may be used as the acrylic wetting agent. Examples of commercially available products include "MODAFLOW AQ3025" manufactured by Allnex and "POLYFLOW WS" manufactured by Kyoeisha Chemical Co., Ltd.
[0030] The silicone wetting agent is a compound having a siloxane skeleton. Either a synthetic product or a commercially available product may be used as the silicone wetting agent. Examples of commercially available products include "Polyflow KL-401" manufactured by Kyoeisha Chemical Co., Ltd. and "Disparlon LS-460" manufactured by Kusumoto Chemical Co., Ltd.
[0031] The wetting agents may be used alone or in combination of two or more.
[0032] The content of the wetting agent in the heat seal layer is 0.04 parts by mass or more and 1.2 parts by mass or less per 100 parts by mass of the water-dispersible resin from the following viewpoints: The content of the wetting agent in the heat seal layer is 0.04 parts by mass or more, preferably 0.06 parts by mass or more, and more preferably 0.08 parts by mass or more per 100 parts by mass of the water-dispersible resin from the viewpoint of heat sealability, and is 1.2 parts by mass or less, preferably 0.7 parts by mass or less, and more preferably 0.4 parts by mass or less from the viewpoint of blocking resistance.
[0033] The content of the wetting agent in the heat seal layer is preferably 0.01% by mass or more and 3.0% by mass or less from the following viewpoints: From the viewpoint of heat sealability, the content of the wetting agent in the heat seal layer is preferably 0.01% by mass or more, more preferably 0.02% by mass or more, even more preferably 0.03% by mass or more, still more preferably 0.04% by mass or more, even more preferably 0.06% by mass or more, and even more preferably 0.08% by mass or more, and from the viewpoint of blocking resistance, it is preferably 3.0% by mass or less, more preferably 2.0% by mass or less, even more preferably 1.2% by mass or less, still more preferably 1.0% by mass or less, even more preferably 0.7% by mass or less, and even more preferably 0.4% by mass or less.
[0034] According to one embodiment of the present invention, the total content of the acetylene-based wetting agent, the acrylic-based wetting agent, and the silicone-based wetting agent in the wetting agent is preferably 85% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and preferably 100% by mass or less.
[0035] According to another embodiment of the present invention, the content of the acetylene-based wetting agent in the wetting agent is preferably 85% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and preferably 100% by mass or less.
[0036] (Lubricant) From the viewpoint of blocking resistance, the heat seal layer preferably contains a lubricant in addition to the water-dispersible resin and wetting agent. A lubricant is a substance that, when blended into the heat seal layer, can reduce the coefficient of friction of the heat seal layer surface.
[0037] The lubricant is not particularly limited, and examples thereof include waxes, metal soaps, and fatty acid esters. Lubricants may be used alone or in combination. Examples of waxes include natural waxes such as animal- or plant-derived waxes (e.g., beeswax, carnauba wax, etc.), mineral waxes (e.g., microcrystalline wax, etc.), and petroleum wax; and synthetic waxes such as polyolefin wax, paraffin wax, and polyester wax. Examples of metal soaps include calcium stearate, sodium stearate, zinc stearate, aluminum stearate, magnesium stearate, fatty acid sodium soap, potassium oleate soap, potassium castor oil soap, and complexes thereof. Among the above lubricants, carnauba wax and paraffin wax are preferred because they have a relatively low melting point, facilitate the formation of wax components on the coating layer surface, and provide excellent blocking suppression. That is, the lubricant is preferably at least one selected from the group consisting of carnauba wax and paraffin wax. As the carnauba wax, either a synthetic product or a commercially available product may be used, and an example of a commercially available product is Cellosol 524 manufactured by Chukyo Yushi Co., Ltd. As the paraffin wax, either a synthetic product or a commercially available product may be used, and an example of a commercially available product is Hydrin L-700 manufactured by Chukyo Yushi Co., Ltd.
[0038] When the heat seal layer contains a lubricant, the content of the lubricant in the heat seal layer is preferably 0.2 parts by mass or more and 15 parts by mass or less, more preferably 0.5 parts by mass or more, even more preferably 1 part by mass or more, and more preferably 10 parts by mass or less, even more preferably 5 parts by mass or less, relative to 100 parts by mass of the water-dispersible resin binder.
[0039] When the heat seal layer contains a lubricant, the content of the lubricant in the heat seal layer is preferably 0.1% by mass or more and 15% by mass or less, more preferably 0.2% by mass or more, even more preferably 0.5% by mass or more, and more preferably 10% by mass or less, even more preferably 5% by mass or less.
[0040] (Pigment) In this embodiment, the heat-seal layer may contain a pigment in addition to the water-dispersible resin, wetting agent, and, if necessary, lubricant. By containing a pigment, the problem of the coated surface of the heat-seal paper sticking to the uncoated surface of the heat-seal paper and causing peeling (blocking) during production and storage of the heat-seal paper is suppressed, and heat-seal paper with excellent blocking resistance can be obtained.
[0041] Specific examples of pigments include mica, bentonite, kaolin, pyrophyllite, talc, smectite, vermiculite, chlorite, septe chlorite, serpentine, stilpnomelane, montmorillonite, heavy calcium carbonate (ground calcium carbonate), light calcium carbonate (synthetic calcium carbonate), composite synthetic pigments of calcium carbonate and other hydrophilic organic compounds, satin white, lithopone, titanium dioxide, silica, barium sulfate, calcium sulfate, alumina, aluminum hydroxide, zinc oxide, magnesium carbonate, silicates, colloidal silica, hollow or solid organic pigment plastic pigments, binder pigments, plastic beads, microcapsules, etc. These may be used alone or in combination of two or more.
[0042] Specific examples of mica include synthetic mica (e.g., swellable synthetic mica), white mica (muscovite), sericite (sericite), phloxopite, biotite (biotite), fluorphlogopite (artificial mica), red mica, soda mica, vanadium mica, illite, zinc mica, paragonite, brittle mica, etc. Specific examples of bentonite include montmorillonite.
[0043] Specific examples of kaolin include various types of kaolin such as kaolin, calcined kaolin, structured kaolin, and delaminated kaolin.
[0044] Among these, it is particularly preferable to include at least one selected from the group consisting of calcium carbonate and kaolin, from the viewpoint of blocking resistance.
[0045] When the heat seal layer contains a pigment, the content of the pigment in the heat seal layer is preferably 10 parts by mass or more and 200 parts by mass or less relative to 100 parts by mass of the water-dispersible resin from the following viewpoints: From the viewpoint of blocking resistance, the content of the pigment in the heat seal layer is preferably 10 parts by mass or more, more preferably 20 parts by mass or more, even more preferably 30 parts by mass or more, and still more preferably 40 parts by mass or more relative to 100 parts by mass of the water-dispersible resin, while from the viewpoint of heat sealability, it is preferably 200 parts by mass or less, more preferably 150 parts by mass or less, and even more preferably 120 parts by mass or less.
[0046] When the heat seal layer contains a pigment, the content of the pigment in the heat seal layer is preferably 5% by mass or more and 70% by mass or less from the following viewpoints: from the viewpoint of blocking resistance, the content of the pigment in the heat seal layer is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 20% by mass or more, and still more preferably 25% by mass or more, and from the viewpoint of heat sealability, it is preferably 70% by mass or less, more preferably 60% by mass or less, and even more preferably 50% by mass or less.
[0047] (Other Components) The heat seal layer may contain other components in addition to the water-dispersible resin, wetting agent, lubricant, and pigment. Examples of other components include silane coupling agents, antifoaming agents, viscosity modifiers, and colorants such as coloring dyes. When the heat seal layer contains the other components, the content of the other components is not particularly limited, but is preferably 0.01 parts by mass or more and 5 parts by mass or less, more preferably 3 parts by mass or less, even more preferably 1 part by mass or less, and more preferably 0.1 parts by mass or more, relative to 100 parts by mass of the water-dispersible resin.
[0048] [Basis Weight, Thickness, and Physical Properties of Heat Seal Paper] (Basis Weight) The basis weight of the heat seal paper is not particularly limited, but is preferably 50 g / m from the following viewpoints: 2 140g / m or more 2 The basis weight of the heat seal paper is preferably 50 g / m2 or less from the viewpoint of obtaining the desired strength. 2 More preferably, 55 g / m 2 More preferably, 60 g / m 2 From the viewpoint of ease of manufacturing the heat seal paper and bag-making processability, it is preferably 140 g / m 2 or less, more preferably 130 g / m 2 More preferably 120 g / m or less 2 The basis weight of the heat seal paper of this embodiment is measured in accordance with JIS P 8124:2011.
[0049] (Thickness) The thickness of the heat seal paper (paper thickness) is not particularly limited, but is preferably 60 μm or more and 220 μm or less from the following viewpoints. From the viewpoint of obtaining the desired strength, the thickness of the heat seal paper (paper thickness) is preferably 60 μm or more, more preferably 80 μm or more, and even more preferably 100 μm or more. From the viewpoint of ease of manufacturing the heat seal paper and bag-making processability, the thickness is preferably 220 μm or less, more preferably 200 μm or less, and even more preferably 180 μm or less. When the thickness is within the above preferred range, the heat seal paper of this embodiment is suitable for use in packaging bags. The thickness of the heat seal paper is measured in accordance with JIS P 8118:2014.
[0050] (Density) The density of the heat seal paper is not particularly limited, but is preferably 0.3 g / cm from the following viewpoints: 3 1.0g / cm or more 3 The density of the heat seal paper is preferably 0.3 g / cm or less from the viewpoint of obtaining a desired strength. 3 More preferably, 0.5 g / cm 3 From the viewpoint of ease of manufacturing the heat seal paper and bag-making processability, it is preferably 1.0 g / cm 3 or less, more preferably 0.9 g / cm 3 More preferably 0.75 g / cm or less 3 The density of the heat seal paper is calculated from the basis weight and thickness of the paper substrate obtained by the above-mentioned measurement method.
[0051] (Oken Smoothness) From the viewpoint of blocking resistance, the heat seal paper of this embodiment preferably has an Oken Smoothness of 50 seconds or less, more preferably 30 seconds or less, and even more preferably 10 seconds or less on the uncoated side. While there is no particular lower limit, it is preferably 1 second or more. The Oken Smoothness of the heat seal paper is measured in accordance with JIS P 8155:2010. The Oken Smoothness of the uncoated side of the heat seal paper can be controlled by the fiber length and beating degree of the pulp, the pressure treatment in the papermaking process, the Clupak treatment conditions, and the like. For example, the Oken Smoothness tends to decrease when pulp with a long fiber length or a low beating degree is used. Furthermore, the Oken Smoothness tends to decrease when the difference between the production speeds on the inlet and outlet sides of the Clupak treatment device is increased.
[0052] (Surface Roughness (RzJIS)) From the viewpoint of blocking resistance, the heat seal paper of this embodiment has a surface roughness (RzJIS) of 12.0 μm or more on the surface opposite to the surface having the heat seal layer (uncoated surface) of 12.0 μm or more, preferably 12.5 μm or more, and more preferably 13.0 μm or more. There is no particular upper limit, but it is preferably 16.0 μm or less, for example. If the RzJIS of the uncoated surface is equal to or greater than the above-mentioned lower limit, relatively large irregularities will be present on the uncoated surface, which is thought to suppress blocking. The surface roughness (RzJIS) of the uncoated surface of the heat seal paper is measured in accordance with JIS B 0601:2013. The surface roughness (RzJIS) of the uncoated surface of the heat seal paper can be controlled by the fiber length and beating degree of the pulp, the pressure treatment in the papermaking process, the conditions of the Clupak treatment, etc. For example, the use of pulp with long fiber length or pulp with a low degree of beating tends to increase the surface roughness (RzJIS). Furthermore, increasing the difference between the production speeds on the inlet and outlet sides of the Clupak processing device also tends to increase the surface roughness (RzJIS). In this specification, the surface roughness (RzJIS) of the surface of the heat seal paper opposite to the surface having the heat seal layer is determined in accordance with JIS B 0601:2013 by measuring the linear roughness in the MD and CD directions, and is the arithmetic mean of the ten-point average roughness in the MD and the ten-point average roughness in the CD, specifically, the value measured by the method described in the Examples.
[0053] (Arithmetic mean roughness (Ra)) From the viewpoint of blocking resistance, the heat seal paper of this embodiment preferably has an arithmetic mean roughness (Ra) of 2.0 μm or more on the uncoated surface, more preferably 2.5 μm or more, and even more preferably 3.0 μm or more. There is no particular upper limit, but for example, it is preferably 5.0 μm or less. The arithmetic mean roughness (Ra) of the uncoated surface of the heat seal paper is measured in accordance with JIS B 0601:2013. The arithmetic mean roughness (Ra) of the uncoated surface of the heat seal paper can be controlled by the fiber length and beating degree of the pulp, the pressure treatment in the papermaking process, the conditions of the Clupak treatment, etc. The tendency is similar to that of the surface roughness (RzJIS). In this specification, the arithmetic mean roughness (Ra) of the surface of the heat seal paper opposite to the surface having the heat seal layer is the arithmetic mean of the arithmetic mean roughness in the MD direction and the arithmetic mean roughness in the CD direction obtained by measuring the line roughness in the MD direction and the CD direction in accordance with JIS B 0601:2013, specifically the value measured by the method described in the Examples. Note that although there is orientation in the paper substrate, RzJIS and Ra are taken as the arithmetic mean of the measured values in the MD direction and the measured values in the CD direction because blocking is a phenomenon that occurs over the entire uncoated surface.
[0054] (Heat seal peel strength) The heat seal paper of this embodiment has a heat seal layer peel strength of preferably 6.0 N / 15 mm or more and 12.0 N / 15 mm or less, more preferably 6.5 N / 15 mm or more, even more preferably 7.0 N / 15 mm or more, and more preferably 11.0 N / mm or less, even more preferably 10.0 N / 15 mm or less. The peel strength of the heat seal layer is the peel strength when the heat seal layers are heat-sealed together under conditions of 160°C, 0.3 MPa, and 0.5 seconds, and is specifically a value measured by the method described in the Examples below. The peel strength can be adjusted by selecting the glass transition temperature and type of the water-dispersible resin and the type and amount of the wetting agent.
[0055] <Method for producing heat-seal paper> The method for producing heat-seal paper of this embodiment is not particularly limited. For example, it includes a coating step of applying a heat-seal layer coating liquid to one side (preferably the wire side (highly smooth side)) of the stretched paper, which is the paper substrate. The heat-seal layer coating liquid (heat-seal layer paint) may be applied two or more times.
[0056] When forming multiple heat-seal layers on a paper substrate, a method of forming the heat-seal layers sequentially is preferred, but this is not limiting, and a simultaneous multi-layer coating method may also be adopted. The simultaneous multi-layer coating method is a method in which multiple types of coating liquids are separately ejected from slit nozzles to form a liquid laminate, which is then coated on the paper substrate to simultaneously form multiple heat-seal layers.
[0057] There are no particular limitations on the coating equipment used to apply the heat seal layer coating liquid to the paper substrate, and known equipment may be used, such as a blade coater, a bar coater, an air knife coater, a slit die coater, a gravure coater, a microgravure coater, a roll coater, a size press, a gate roll coater, or a shim sizer.
[0058] The drying equipment for drying the heat-seal layer is not particularly limited, and known equipment can be used. Examples of drying equipment include a hot air dryer, an infrared dryer, a gas burner, and a hot plate. The drying temperature may be appropriately set taking into account the drying time, etc. It is preferable to adjust the conditions for forming the heat-seal layer so that the formation of the heat-seal layer does not affect the surface roughness (RzJIS) of the uncoated side of the paper substrate.
[0059] The solvent for the heat-seal layer coating liquid is not particularly limited, and water or an organic solvent such as ethanol, isopropyl alcohol, methyl ethyl ketone, or toluene can be used. Among these, water is preferred as the dispersion medium for the heat-seal layer coating liquid, from the viewpoint of avoiding the problems of volatile organic solvents. In other words, the heat-seal layer coating liquid is preferably an aqueous composition for a heat-seal layer.
[0060] The solid content (solid content concentration) of the heat seal layer coating liquid is not particularly limited and may be appropriately selected from the viewpoints of coatability and ease of drying, but is preferably 20% by mass or more and 80% by mass or less, more preferably 25% by mass or more, even more preferably 30% by mass or more, and more preferably 65% by mass or less, even more preferably 50% by mass or less.
[0061] The basis weight of the heat seal layer (when the heat seal layer is provided by coating, the coating amount (after drying)) is preferably 7 g / m 2 21g / m or more 2 More preferably, 8 g / m or less. 2 More preferably, 9 g / m 2 More preferably, it is 19 g / m or more. 2 More preferably, 17 g / m or less 2 The heat seal layer may be one layer or two or more layers. When the heat seal layer is two or more layers, the above coating amount represents the total coating amount.
[0062] [Uses] The heat seal paper according to this embodiment can be suitably used as a packaging bag for food, household goods, daily necessities (soap, diapers), etc. Therefore, the present invention also provides a packaging bag using the above heat seal paper.
[0063] The features of the present invention will be explained in more detail below with reference to examples and comparative examples. The materials, amounts used, ratios, treatment details, treatment procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below. Furthermore, unless otherwise specified, the operations in the examples and comparative examples were carried out at room temperature (20-25°C) and normal humidity (40-50% RH).
[0064] Example 1 Preparation of Heat-Seal Layer Coating Fluid 100 parts by mass (solids content equivalent) of an aqueous dispersion of a styrene-butadiene copolymer (Nipol Latex LX407S12, manufactured by Zeon Corporation, solids content 46% by mass, glass transition temperature 18°C), 3 parts by mass (solids content equivalent) of a lubricant (Hydrin L-700, manufactured by Chukyo Yushi Co., Ltd., solids content 30% by mass), 0.05 parts by mass (active ingredient equivalent) of an acetylene glycol wetting agent (Meisei Chemical Industry Co., Ltd., Meikasurf S-28, active ingredient 20% by mass), and 0.4 parts by mass (active ingredient equivalent) of an antifoaming agent (SN0215, manufactured by San Nopco Ltd., active ingredient 15% by mass), were mixed, and water was added thereto to give a solids content of 38% by mass, followed by stirring to prepare a heat-seal layer coating fluid (concentration 38% by mass). (Coating of heat seal layer coating liquid) The obtained heat seal layer coating liquid was applied to a sheet of paper containing 100% by mass of softwood unbleached kraft pulp (NUKP) and having a basis weight of 100 g / m 2 , thickness 150 μm, density 0.67 g / cm 3 The coated surface of the paper substrate (stretched paper) had a Stockigt sizing degree of 73 seconds on the coated surface (wire surface, high smoothness), a Stockigt sizing degree of 79 seconds on the uncoated surface (felt surface, low smoothness), and a surface roughness (RzJIS) of 14.9 μm on the uncoated surface (felt surface, low smoothness). The coating weight of the heat seal layer after drying was 14 g / m. 2 The mixture was coated with a bar coater so that the thickness of the coating was as follows: and then dried at 140° C. for 25 seconds to form a heat seal layer, thereby obtaining a heat seal paper.
[0065] [Example 2] A heat seal paper was obtained in the same manner as in Example 1, except that in the preparation of the heat seal layer coating liquid in Example 1, the amount of the acetylene glycol-based wetting agent added was changed to 0.1 parts by mass (in terms of active ingredient).
[0066] [Example 3] A heat seal paper was obtained in the same manner as in Example 1, except that in the preparation of the heat seal layer coating liquid in Example 1, the amount of the acetylene glycol-based wetting agent added was changed to 0.2 parts by mass (in terms of active ingredient).
[0067] [Example 4] A heat seal paper was obtained in the same manner as in Example 1, except that in the preparation of the heat seal layer coating liquid in Example 1, the amount of the acetylene glycol-based wetting agent added was 1.0 part by mass (in terms of active ingredient).
[0068] [Example 5] A heat seal paper was obtained in the same manner as in Example 3, except that in the preparation of the heat seal layer coating liquid in Example 3, the acetylene glycol-based wetting agent was changed to an acrylic-based wetting agent (MODAFLOW AQ3025, manufactured by Allnex, active ingredient 25% by mass).
[0069] [Example 6] A heat-sealable paper was obtained in the same manner as in Example 3, except that in the preparation of the heat-sealable layer coating liquid in Example 3, the acetylene glycol-based wetting agent was changed to a silicone-based wetting agent (manufactured by Kyoeisha Chemical Co., Ltd., Polyflow KL-401, active ingredient 100% by mass).
[0070] [Example 7] In the coating of the heat seal layer coating liquid in Example 3, the paper substrate was made of 100% softwood unbleached kraft pulp with a basis weight of 88 g / m 2 , thickness 135 μm, density 0.65 g / cm 3 A heat-sealable paper was obtained in the same manner as in Example 3, except that the coated surface (wire surface, high smoothness surface) was changed to a stretched paper with a Stockigt sizing degree of 75 seconds, the uncoated surface (felt surface, low smoothness surface) to a Stockigt sizing degree of 70 seconds, and the uncoated surface (felt surface, low smoothness surface) to a surface roughness (RzJIS) of 13.8 μm.
[0071] [Example 8] In the coating of the heat seal layer coating liquid in Example 3, the paper substrate was made of 100% softwood unbleached kraft pulp with a basis weight of 88 g / m 2 , thickness 135 μm, density 0.65 g / cm 3 A heat-sealable paper was obtained in the same manner as in Example 3, except that the coated surface (felt surface, low smoothness surface) was changed to a stretched paper with a Stockigt sizing degree of 60 seconds, the uncoated surface (wire surface, high smoothness surface) to a Stockigt sizing degree of 60 seconds, and the uncoated surface to a surface roughness (RzJIS) of 13.4 μm.
[0072] Comparative Example 1 A heat seal paper was obtained in the same manner as in Example 1, except that the acetylene glycol-based wetting agent was not used in preparing the heat seal layer coating liquid.
[0073] Comparative Example 2 A heat-sealable paper was obtained in the same manner as in Example 1, except that in the preparation of the heat-sealable layer coating liquid in Example 1, the amount of the acetylene glycol-based wetting agent added was changed to 0.03 parts by mass (in terms of active ingredient).
[0074] Comparative Example 3 A heat-sealable paper was obtained in the same manner as in Example 1, except that in the preparation of the heat-sealable layer coating liquid in Example 1, the amount of the acetylene glycol-based wetting agent added was changed to 1.5 parts by mass (in terms of active ingredient).
[0075] [Comparative Example 4] In the coating of the heat seal layer coating liquid of Example 3, 100% by mass of unbleached softwood kraft pulp and a basis weight of 100 g / m 2 , thickness 155 μm, density 0.65 g / cm 3 A heat seal paper was obtained in the same manner as in Example 3, except that the unbleached light packaging paper was used, with a Stockigt sizing degree of 36 seconds on the coated side (wire side, high smoothness side), a Stockigt sizing degree of 30 seconds on the uncoated side (felt side, low smoothness side), and a surface roughness (RzJIS) of 10.4 μm on the uncoated side (felt side, low smoothness side).
[0076] Comparative Example 5 A heat-sealable paper was obtained in the same manner as in Example 3, except that in the preparation of the heat-sealable layer coating solution in Example 3, the aqueous dispersion of a styrene-butadiene copolymer was changed to an aqueous dispersion of a styrene-butadiene copolymer (Narstar SR-110, manufactured by Nippon A&L Co., Ltd., solid content 46% by mass, glass transition temperature -27°C).
[0077] <Evaluation> The paper substrates and the heat seal papers produced in the examples and comparative examples were measured or evaluated for the following items.
[0078] (Basis Weight) The basis weight of the paper base material and the heat seal paper was measured in accordance with JIS P 8124:2011.
[0079] (Thickness) The thickness of the paper substrate and the heat seal paper was measured in accordance with JIS P 8118: 2014. (Density) The density of the paper substrate and the heat seal paper was calculated from the basis weight and thickness obtained by the above-mentioned measurement method.
[0080] (Stockigt Sizing Degree) The Stockigt sizing degree of the coated and uncoated surfaces of the heat seal paper was measured in accordance with JIS P 8122:2004.
[0081] (Oken Smoothness) The uncoated surface of the heat seal paper was subjected to Oken Smoothness measurement in accordance with JIS P 8155:2010.
[0082] (Ten-point average roughness (RzJIS)) The ten-point average roughness (surface roughness (RzJIS)) of the uncoated surface of the heat seal paper was measured in accordance with JIS B 0601:2013. For the measurement, a "One-shot 3D shape measuring instrument VR-3000 / VR-3200" manufactured by KEYENCE Corporation and the analysis application "VR-H2A" built into the VR-3000 were used. The observation conditions were a magnification of 80x and a field of view of 3.8 mm x 2.9 mm. Linear roughness measurements were performed in the MD and CD directions at any five locations on the sample, and the arithmetic mean of the ten-point average roughness measurements in the MD direction and the ten-point average roughness measurements in the CD direction at the five locations was taken as the ten-point average roughness RzJIS of the sample. Specifically, a sample approximately A4 size was cut from heat seal paper, and the uncoated side of the sample was placed facing up along the edge of the stage of the VR-3200 so that the CD direction of the sample coincided with the depth direction of the stage. Measurements were performed using autofocus at 80x magnification, resulting in an observation image measuring 3.8 mm horizontal x 2.9 mm vertical. The horizontal direction of the obtained observation image corresponds to the MD direction of the sample, and the vertical direction corresponds to the CD direction of the sample. A horizontal line (a straight line in the horizontal direction) was selected at any position on the obtained observation image, and line roughness analysis was performed, and the ten-point average roughness in the MD direction was automatically measured. Furthermore, a vertical line (a straight line in the vertical direction) was selected at any position on the obtained observation image, and line roughness analysis was performed, and the ten-point average roughness in the CD direction was automatically measured. The same measurements as above were carried out by changing the measurement position, and the ten-point average roughness in the MD direction and the ten-point average roughness in the CD direction were measured at any five points on the sample, and the arithmetic mean of these measurement values was calculated to obtain the ten-point average roughness (RzJIS) of the sample.
[0083] (Arithmetic mean roughness (Ra)) The arithmetic mean roughness (Ra) of the uncoated surface of the heat seal paper was measured in accordance with JIS B 0601: 2013. Using the same measuring equipment and observation conditions as in the ten-point mean roughness measurement, line roughness analysis was performed in the MD and CD directions at any five locations on the sample, and the arithmetic mean roughness (Ra) of the sample was calculated by taking the arithmetic mean roughness measurement values in the MD direction and the arithmetic mean roughness measurement values in the CD direction for the five locations.
[0084] (Heat seal peel strength) Two sheets of heat seal paper were stacked with the heat seal layers facing each other, and heat sealed using a heat seal tester (TP-701-B, manufactured by Tester Sangyo Co., Ltd.) under conditions of 160°C, 0.3 MPa, and 0.5 seconds. The heat-sealed test piece was left to stand for 4 hours or more in a room at a temperature of 23°C ± 1°C and a relative humidity of 50% ± 2%. Subsequently, the heat-sealed test piece was cut to a width of 15 mm and subjected to T-peel at a tensile speed of 300 mm / min using a tensile tester, and the recorded maximum load was taken as the heat seal peel strength.
[0085] (Blocking Resistance) Heat seal paper was cut into 9 cm squares, stacked so that the coated surface and the uncoated surface faced each other, and pressed at a temperature of 40°C and a pressure of 46 kg / cm using a press (Mini Test Press-10, model MP-SNH, manufactured by Toyo Seiki Seisaku-sho, Ltd.). 2 The paper was pressed with a pressure of 1000 W and kept in that state for 15 hours. After 15 hours, the paper was removed from the press and the sample was peeled off by hand. The condition of the sample after peeling was checked and evaluated according to the following criteria. If it is rated A or B, it can be judged to be usable for practical use. [Evaluation criteria] A: No paper peeling or fluffing. B: No paper peeling, but some fluffing. C: Paper peeling.
[0086]
[0087]
[0088] (Table notes) S12: LX407S12 manufactured by Nippon Zeon Co., Ltd. SBR: Styrene-butadiene copolymer SR-110: Nalstar SR-110 manufactured by Nippon A&L Co., Ltd.
[0089] Tables 1-1 and 1-2 show that heat-sealable papers having a heat-sealable layer on one side of a paper substrate, the heat-sealable layer containing a water-dispersible resin and a wetting agent, the water-dispersible resin containing a water-dispersible resin with a glass transition temperature of 0°C or higher, the wetting agent content being 0.04 to 1.2 parts by mass per 100 parts by mass of the water-dispersible resin, and the surface roughness (RzJIS) of the uncoated side being 12.0 μm or higher, exhibit excellent heat-sealability and blocking resistance (Examples 1 to 8). Furthermore, heat-sealable papers in which the water-dispersible resin contains a styrene-butadiene copolymer with a glass transition temperature of 0°C or higher and the wetting agent contains an acetylene-based wetting agent exhibit even better heat-sealability (Compare Example 3 with Examples 5 and 6). In contrast, heat-sealable paper containing a water-dispersible resin but no wetting agent in the heat-sealable layer, and heat-sealable paper containing a water-dispersible resin and a wetting agent but with a wetting agent content of less than 0.04 parts by mass (0.03 parts by mass) per 100 parts by mass of the water-dispersible resin, exhibited poor heat-sealability (Comparative Examples 1 and 2). Heat-sealable paper containing a water-dispersible resin and a wetting agent but with a wetting agent content of more than 1.2 parts by mass (1.5 parts by mass) per 100 parts by mass of the water-dispersible resin exhibited poor blocking resistance (Comparative Example 3). Heat-sealable paper with a surface roughness (RzJIS) of less than 12.0 μm (10.4 μm) on the uncoated side also exhibited poor blocking resistance (Comparative Example 4). Furthermore, heat-sealable paper containing a water-dispersible resin and a wetting agent in the heat-sealable layer but with a water-dispersible resin with a glass transition temperature of less than 0°C (-27°C) also exhibited poor blocking resistance (Comparative Example 5).
Claims
1. A heat seal paper having a heat seal layer on one side of a paper base material, the heat seal layer comprising a water-dispersible resin and a wetting agent, the water-dispersible resin comprising a water-dispersible resin having a glass transition temperature of 0°C or higher, the content of the wetting agent being 0.04 parts by mass or more and 1.2 parts by mass or less per 100 parts by mass of the water-dispersible resin, and the surface roughness (RzJIS) of the surface of the heat seal paper opposite to the surface having the heat seal layer is 12.0 μm or more.
2. The heat seal paper according to claim 1, wherein the wetting agent comprises at least one selected from the group consisting of acetylene-based wetting agents, acrylic-based wetting agents, and silicone-based wetting agents.
3. The heat-sealable paper according to claim 1 or 2, wherein the water-dispersible resin comprises a styrene-butadiene copolymer.
4. The heat seal paper according to any one of claims 1 to 3, wherein the water-dispersible resin comprises a styrene-butadiene copolymer and the wetting agent comprises an acetylene-based wetting agent.
5. Basis weight: 50g / m 2 140g / m or more 2 The heat seal paper according to any one of claims 1 to 4, wherein:
6. The heat sealable paper according to any one of claims 1 to 5, wherein the paper substrate is a stretch paper.
7. The basis weight of the heat seal layer is 7 g / m 2 21g / m or more 2 The heat seal paper according to any one of claims 1 to 6, wherein:
8. A heat seal paper according to any one of claims 1 to 7, in which the heat seal peel strength when the heat seal layers are heat sealed together under conditions of 160°C, 0.3 MPa, and 0.5 seconds is 6.0 N / 15 mm or more.
9. A packaging bag using the heat seal paper according to any one of claims 1 to 8.
Citation Information
Patent Citations
Ink jet recording paper
JP2009208471A
Paper-made barrier material
JP2019173258A
Heat seal paper
JP2022175023A
Heat-seal paper and packaging bags
JP7070785B1
Paper barrier material
WO2019189229A1