Resin composition, diamine compound, cured product, multilayer body, method for producing cured product, method for producing multilayer body, method for producing semiconductor device, and semiconductor device
The resin composition with specific repeating units and a novel diamine compound addresses the challenge of maintaining insulation and adhesion in semiconductor devices, achieving improved reliability and chemical resistance by reducing water penetration and unpolymerized areas.
Patent Information
- Application Number
- PCT/JP2024/010958
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-03
AI Technical Summary
There is a need for resin compositions that maintain insulation properties and adhesion over a long period, particularly in semiconductor devices, where existing materials face challenges in reliability and chemical resistance.
A resin composition containing specific repeating units with ethylenically unsaturated bonds and a low phenolic hydroxyl group content, along with a novel diamine compound, is used to form a cured product with improved reliability and chemical resistance, suitable for semiconductor device applications.
The resin composition achieves excellent reliability and chemical resistance, reducing water penetration and unpolymerized areas, leading to enhanced insulation and mechanical properties in semiconductor devices.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Resin composition, diamine compound, cured product, laminate, method for producing cured product, method for producing laminate, method for producing semiconductor device, and semiconductor device
[0001] The present invention relates to a resin composition, a diamine compound, a cured product, a laminate, a method for producing a cured product, a method for producing a laminate, a method for producing a semiconductor device, and a semiconductor device.
[0002] Nowadays, resin materials produced from resin compositions containing resins are being utilized in various fields. For example, cyclized resins such as polyimides are used in a variety of applications due to their excellent heat resistance and insulating properties. Examples of such applications include, but are not limited to, insulating films, sealing materials, or protective films for semiconductor devices used for packaging. They are also used as base films or coverlays for flexible substrates.
[0003] For example, in the above-mentioned applications, a cyclized resin such as polyimide is used in the form of a resin composition containing the cyclized resin. Such a resin composition is applied to a substrate, for example, by coating, to form a photosensitive film, and then, as necessary, exposure, development, heating, etc., can be performed to form a cured product on the substrate. Since the resin composition can be applied by known coating methods, for example, it can be said to have excellent manufacturing adaptability, such as a high degree of design freedom in the shape, size, application position, etc., when applying the resin composition. In addition to the high performance of polyimide, from the perspective of such excellent manufacturing adaptability, the industrial application development of the above-mentioned resin composition is increasingly expected.
[0004] For example, Patent Document 1 describes a photosensitive polyimidesiloxane obtained by polymerizing and imidizing (a) 85 to 99 mol % of a diamine compound having a specific structure and at least two photosensitive groups, (b) 15 to 1 mol % of a diaminopolysiloxane having a specific structure, and (c) a tetracarboxylic dianhydride having a specific structure, and a composition containing the same. Patent Document 2 describes a negative photosensitive resin composition containing (A) a polyimide having a double bond in the side chain, (B) a crosslinking agent including a (meth)acrylate compound having a fluorene skeleton, and (C) a polymerization initiator.
[0005] JP 2006-083307 A JP 2022-135427 A
[0006] It is required that the cured product obtained from the resin composition can maintain its insulating properties for a long period of time. In the present invention, the ability to maintain adhesion for a long period of time is also referred to as "excellent reliability."
[0007] The present invention aims to provide a resin composition that can give a cured product with excellent reliability, a cured product obtained by curing the composition, a laminate including the cured product, a method for producing the cured product, a method for producing the laminate, a method for producing a semiconductor device including the method for producing the cured product, and a semiconductor device including the cured product. Another object of the present invention is to provide a novel diamine compound.
[0008] Representative embodiments of the present invention are shown below: <1> A resin composition comprising: a resin that contains a repeating unit represented by the following formula (1-1), that contains a group having an ethylenically unsaturated bond, and that has a phenolic hydroxyl group content of 0.250 mmol / g or less; and a polymerizable compound having an ethylenically unsaturated bond: In formula (1-1), X 1 represents a tetravalent organic group, Y 1 <2> The resin composition according to <1>, wherein the resin is a resin containing a repeating unit represented by the following formula (1-2) as the repeating unit represented by the formula (1-1): In formula (1-2), X 1 represents a tetravalent organic group, Y 2represents a group containing a group represented by the following formula (2-1). In formula (2-1), R 1 and R 2 each independently represent a group having an ethylenically unsaturated bond, L represents a single bond or a divalent linking group not containing an imide bond, and each * represents a bonding site with another structure. <3> The resin composition according to <1> or <2>, wherein the resin contains a group having a vinylphenyl group as the group having an ethylenically unsaturated bond. <4> A resin composition comprising: a resin containing a repeating unit represented by the following formula (1-3) and containing a vinylphenyl group; and a polymerizable compound having an ethylenically unsaturated bond: In formula (1-3), X 1 represents a tetravalent organic group, Y 3 represents a group containing a group represented by the following formula (2-2). In formula (2-2), R 1 and R 2 each independently represents a group having an ethylenically unsaturated bond, L represents a single bond, —C(CH 3 ) 2 -, or -C(CF 3 ) 2 <5> The resin composition according to any one of <1> to <4>, wherein the resin has a structure represented by any one of the following formulas (3-1) to (3-3): In formula (3-1), X 31 represents a tetravalent organic group, Y 31 represents a divalent organic group, R 31 represents a group having an ethylenically unsaturated bond, and * represents a bonding site with another structure. 31 represents a tetravalent organic group, Y 31 represents a divalent organic group, R 31 represents a group having an ethylenically unsaturated bond, and * represents a bonding site with another structure. 31 represents a tetravalent organic group, Y 31 represents a divalent organic group, R 32 and R 33 each independently represents —OH or a monovalent organic group, and R 32 and R33 at least one of the groups is a group having an ethylenically unsaturated bond, and * represents a bonding site with another structure. <6> The resin composition according to any one of <1> to <5>, wherein the resin is a resin having a rate of change in imide group value calculated by the following formula before and after heating at 350°C and 1 atmosphere for 1 hour of 25% or less: Rate of change (%) = (Im2 - Im1) × 100 / Im1, where Im1 is the imide group value (mmol / g) before heating, and Im2 is the imide group value (mmol / g) after heating at 350°C and 1 atmosphere for 1 hour. <7> The X 1 is an organic group containing a structure in which two or more hydrogen atoms have been removed from a structure represented by any one of formulas (V-1) to (V-4). The resin composition according to any one of <1> to <6>. In formula (V-2), R X1 are each independently a hydrogen atom, an alkyl group, or a halogenated alkyl group. X2 and R X3 each independently represents a hydrogen atom or a substituent, R X2 and R X3 may be bonded to form a ring structure. <8> The resin composition according to any one of <1> to <7>, containing an azole compound. <9> A diamine compound represented by the following formula (4-1): In formula (4-1), R 3 and R 4 each independently represents a group having an ethylenically unsaturated bond, R 3 and R 4 At least one of the groups has an aromatic hydrocarbon group, and L is a single bond, -C(CH 3 ) 2 - or - C(CF 3 ) 2 <10> The above R 3 and R 4each independently having a vinylphenyl group. <11> A resin composition comprising: a resin that is a reaction product of the diamine compound according to <9> or <10> with a compound or derivative thereof having two or more carboxy groups and two or more carboxylic anhydride groups in total; and a polymerizable compound having an ethylenically unsaturated bond. <12> The resin composition according to any one of <1> to <11>, used for forming an interlayer insulating film for a redistribution layer. <13> A cured product obtained by curing the resin composition according to any one of <1> to <12>. <14> A laminate comprising two or more layers made of the cured product according to <13>, and a metal layer between any two adjacent layers made of the cured product. <15> A method for producing a cured product, comprising a film-forming step of applying the resin composition according to any one of <1> to <12> onto a substrate to form a film. <16> A method for producing a cured product according to <15>, comprising an exposure step of selectively exposing the film to light and a development step of developing the film with a developer to form a pattern. <17> A method for producing the cured product according to <15> or <16>, comprising a heating step of heating the film at 50 to 450°C. <18> A method for producing a laminate, comprising the method for producing a cured product according to any one of <15> to <17>. <19> A method for producing a semiconductor device, comprising the method for producing a cured product according to any one of <15> to <17>. <20> A semiconductor device, comprising the cured product according to <13>.
[0009] According to the present invention, there are provided a resin composition which can give a cured product with excellent reliability, a cured product obtained by curing the composition, a laminate including the cured product, a method for producing the cured product, a method for producing the laminate, a method for producing a semiconductor device including the method for producing the cured product, and a semiconductor device including the cured product. Also, according to the present invention, there is provided a novel diamine compound.
[0010] The following describes the main embodiments of the present invention. However, the present invention is not limited to the explicitly described embodiments. In this specification, a numerical range expressed using the symbol "to" means a range that includes the numerical values before and after "to" as the lower and upper limits, respectively. In this specification, the term "process" refers not only to an independent process but also to a process that cannot be clearly distinguished from other processes as long as the process achieves its intended effect. In the description of a group (atomic group), a notation that does not specify whether it is substituted or unsubstituted encompasses both unsubstituted groups (atomic groups) and substituted groups (atomic groups). For example, the term "alkyl group" encompasses not only unsubstituted alkyl groups (unsubstituted alkyl groups) but also substituted alkyl groups (substituted alkyl groups). In this specification, unless otherwise specified, "exposure" includes not only exposure using light but also exposure using particle beams such as electron beams and ion beams. In addition, examples of light used for exposure include actinic rays or radiation such as the bright line spectrum of a mercury lamp, far ultraviolet light typified by excimer lasers, extreme ultraviolet light (EUV light), X-rays, and electron beams. As used herein, "(meth)acrylate" refers to either or both of "acrylate" and "methacrylate," "(meth)acrylic" refers to either or both of "acrylic" and "methacrylic," and "(meth)acryloyl" refers to either or both of "acryloyl" and "methacryloyl." In the structural formulae herein, Me represents a methyl group, Et represents an ethyl group, Bu represents a butyl group, and Ph represents a phenyl group. As used herein, the term "total solid content" refers to the total mass of all components of the composition excluding the solvent. Furthermore, as used herein, the term "solid content concentration" refers to the mass percentage of the components other than the solvent relative to the total mass of the composition. As used herein, the weight average molecular weight (Mw) and number average molecular weight (Mn) are values measured using gel permeation chromatography (GPC) and are defined as polystyrene equivalent values, unless otherwise specified.In this specification, the weight-average molecular weight (Mw) and number-average molecular weight (Mn) can be determined, for example, by using an HLC-8220GPC (manufactured by Tosoh Corporation) and guard columns HZ-L, TSKgel Super HZM-M, TSKgel Super HZ4000, TSKgel Super HZ3000, and TSKgel Super HZ2000 (all manufactured by Tosoh Corporation) connected in series. Unless otherwise specified, these molecular weights are measured using THF (tetrahydrofuran) as the eluent. However, when THF is not suitable as the eluent, for example, due to low solubility, NMP (N-methyl-2-pyrrolidone) can also be used. Furthermore, unless otherwise specified, detection in GPC measurement is assumed to be performed using a UV (ultraviolet) detector at a wavelength of 254 nm. In this specification, when the positional relationship of each layer constituting a laminate is described as "above" or "below," it is sufficient that another layer is above or below the reference layer among the multiple layers being considered. In other words, a third layer or element may be interposed between the reference layer and the other layer, and the reference layer and the other layer do not need to be in contact with each other. Unless otherwise specified, the direction in which layers are stacked on the substrate is referred to as "above." Alternatively, if a resin composition layer is present, the direction from the substrate to the resin composition layer is referred to as "above," and the opposite direction is referred to as "below." Note that such vertical directions are defined for convenience in this specification, and in actual embodiments, the "above" direction in this specification may differ from the vertically upward direction. In this specification, unless otherwise specified, the composition may contain two or more compounds corresponding to each component contained in the composition. Furthermore, unless otherwise specified, the content of each component in the composition means the total content of all compounds corresponding to that component. In this specification, unless otherwise specified, the temperature is 23° C., the atmospheric pressure is 101,325 Pa (1 atmosphere), and the relative humidity is 50% RH. In this specification, a combination of preferred embodiments is a more preferred embodiment.
[0011] (Resin Composition) A resin composition according to a first aspect of the present invention (hereinafter also simply referred to as the "first resin composition") comprises a resin containing a repeating unit represented by formula (1-1), a group having an ethylenically unsaturated bond, and a phenolic hydroxyl group content of 0.250 mmol / g or less, and a polymerizable compound having an ethylenically unsaturated bond. A resin composition according to a second aspect of the present invention (hereinafter also simply referred to as the "second resin composition") comprises a resin containing a repeating unit represented by formula (1-3) and a vinylphenyl group, and a polymerizable compound having an ethylenically unsaturated bond. A resin composition according to a third aspect of the present invention (hereinafter also simply referred to as the "third resin composition") comprises a resin that is a reaction product of a diamine compound represented by formula (4-1) and a compound having a total of two or more carboxy groups and carboxylic acid anhydride groups, and a polymerizable compound having an ethylenically unsaturated bond. Hereinafter, the first resin composition, the second resin composition, and the third resin composition will be collectively referred to as the "resin composition". Hereinafter, a resin contained in a first resin composition, which contains a repeating unit represented by formula (1-1), contains a group having an ethylenically unsaturated bond, and has a phenolic hydroxyl group content of 0.250 mmol / g or less, is also referred to as a "first specific resin." Hereinafter, a resin contained in a second resin composition, which contains a repeating unit represented by formula (1-3) and contains a vinylphenyl group, is also referred to as a "second specific resin." Hereinafter, a resin contained in a third resin composition, which is a reaction product of a diamine compound represented by formula (4-1) and a compound having a total of two or more carboxy groups and carboxylic acid anhydride groups, is also referred to as a "third specific resin." Hereinafter, when simply referring to a "specific resin," it refers to all of the first specific resin, second specific resin, and third specific resin.
[0012] The resin composition of the present invention is preferably used to form a photosensitive film that is subjected to exposure and development, and more preferably to form a film that is subjected to exposure and development using a developer containing an organic solvent. The resin composition of the present invention can be used to form, for example, an insulating film for a semiconductor device, an interlayer insulating film for a rewiring layer, a stress buffer film, etc., and is preferably used to form an insulating member. The insulating member is a member formed for the purpose of insulating between members intended for electrical conductivity such as wiring. The volume resistivity of the insulating member is 1×10 8 It is preferable that the resistance is Ω cm or more, and 1×10 10 More preferably, it is 1×10 Ω cm or more. 12 It is more preferable that the resistivity is Ω·cm or more. In particular, one preferred embodiment of the present invention is that the resin composition of the present invention is used to form an interlayer insulating film for a redistribution layer. Furthermore, the resin composition of the present invention is preferably used to form a photosensitive film to be subjected to negative development. In the present invention, negative development refers to development in which non-exposed areas are removed by development in exposure and development, and positive development refers to development in which exposed areas are removed by development. As the exposure method, the developer, and the development method, for example, the exposure method described in the exposure step and the developer and development method described in the development step in the description of the method for producing a cured product described below are used.
[0013] The resin composition of the present invention provides a cured product with excellent reliability. The mechanism by which the above effects are obtained is unknown, but is presumed to be as follows.
[0014] The resin contained in the resin composition according to the first aspect has a small content of phenolic hydroxyl groups. The resin contained in the resin composition according to the second aspect has a vinylphenyl group. Since the vinylphenyl group has lower mobility compared to polymerizable groups such as acryloxy groups, it is thought that even in a structure where L described in formula (2-2) is short, it is easy to introduce it into an adjacent structure. The resin contained in the resin composition according to the third aspect is thought to have a smaller content of phenolic hydroxyl groups in the resin by using a specific diamine, compared to when a polymerizable group is later introduced into the phenolic hydroxyl group of a structure derived from a diamine having a phenolic hydroxyl group.
[0015] Although the reason why the use of these resins results in excellent reliability is unclear, it is presumed that the low content of phenolic hydroxyl groups in the resin prevents the movement of groups having ethylenically unsaturated bonds in the resin from being hindered by the phenolic hydroxyl groups in some locations. Furthermore, the polymerization-inhibiting effect of the phenolic hydroxyl groups prevents the polymerization of groups having ethylenically unsaturated bonds from being hindered in the locations where the phenolic hydroxyl groups are present. As a result, polymerization proceeds nearly uniformly in the film made of the resin composition, and the cured product obtained after polymerization is thought to have fewer unpolymerized locations where phenolic hydroxyl groups are present. In other words, the cured product obtained from the resin composition of the present invention is thought to have excellent reliability because penetration of water and the like from such unpolymerized locations is suppressed. Furthermore, the reduction in unpolymerized locations is thought to improve the elongation at break of the resulting cured product. In addition, the use of a resin with a specific structure can reduce the dielectric loss tangent of the resulting cured product. Furthermore, a small content of phenolic hydroxyl groups in the resin may result in effects such as improved chemical resistance of the resulting cured product and improved developability when a film made of the resin composition is subjected to exposure and development.
[0016] However, there is no description of a resin composition that corresponds to the resin composition of the present invention in Patent Documents 1 and 2. Hereinafter, the details of each component included in the present invention will be described.
[0017] <Specific Resin> The first specific resin and the second specific resin are preferably polyimide resins. A polyimide resin refers to a resin containing a plurality of repeating units having an imide bond. In the present invention, an imide bond is a structure represented by -C(=O)N(-*)C(=O)-. * represents a bonding site with another structure. Furthermore, the polyimide resin is preferably a resin having an imide bond in its main chain structure, and more preferably a resin containing an imide ring structure in its main chain structure. An imide ring structure refers to a ring structure containing all of the two carbon atoms and one nitrogen atom in the imide bond as ring members. The imide ring structure is preferably a five-membered ring structure. In the present invention, the "main chain" refers to the relatively longest bonding chain in the resin molecule, and the "side chain" refers to other bonding chains.
[0018] The third specific resin is preferably a polyimide resin, a polyamide resin, or a polyamideimide resin, and more preferably a polyimide resin. A polyamide resin refers to a resin containing a plurality of repeating units having an amide bond. In the present invention, the amide bond is represented by *-NR N -C(=O)-*, and R N represents a hydrogen atom or a monovalent organic group, and * represents a bonding site with a carbon atom. N is preferably a hydrogen atom, an alkyl group or an aryl group, and more preferably a hydrogen atom. The polyamide-imide resin refers to a resin containing a plurality of repeating units having an imide bond and an amide bond.
[0019] [Phenolic Hydroxyl Group Content] The first specific resin has a phenolic hydroxyl group content of 0.250 mmol / g or less. The second specific resin and the third specific resin preferably have a phenolic hydroxyl group content of 0.250 mmol / g or less. In the present invention, a phenolic hydroxyl group refers to a hydroxy group bonded to an aromatic ring structure by a single bond without a linking group. The aromatic ring structure may be an aromatic hydrocarbon ring structure or an aromatic heterocyclic structure. The phenolic hydroxyl group content in the specific resin is preferably 0.200 mmol / g or less, more preferably 0.180 mmol / g or less, even more preferably 0.150 mmol / g or less, and particularly preferably 0.120 mmol / g or less. Here, the lower limit of the phenolic hydroxyl group content is not particularly limited and may be 0 mmol / g (i.e., below the limit of quantitation). The phenolic hydroxyl group content is calculated based on the ratio of 1 mole of resin to 1 mole of resin. 1 The amount of phenolic hydroxyl groups (mmol) can be calculated by dividing the amount (mmol) of phenolic hydroxyl groups measured by H-NMR by the number average molecular weight of the resin. The amount (mmol) of phenolic hydroxyl groups can be calculated by known quantitative NMR. Specifically, it can be measured under the following measurement conditions. - Measurement conditions - 1 H-NMR (BRUKER, AVANCE NEO 400) Analysis software: TopSpin 4.0.7 Solvent: DMSO-d6 Internal standard: 1,3,5-trimethoxybenzene 1 In H-NMR, a specific peak for the proton of the phenolic hydroxyl group is detected near δ(DMSO-d6) = 10 ppm. Also, a specific peak is detected at 6.1 ppm for the internal standard 1,3,5-trimethoxybenzene. The number average molecular weight is obtained as a polystyrene equivalent value measured by gel permeation chromatography (GPC).
[0020] Furthermore, when the above measurement is difficult, the acid value (mg KOH / g) of the resin can be measured by acid value titration, and then the acid value can be converted to mol / g. The proportion of phenolic hydroxyl groups among the acid groups contained in the specific resin can be quantified by NMR, and the proportion can be integrated into the acid value. In acid value titration, the neutralization point can be detected separately from carboxylic acids because they have different pKa.
[0021] [Group Having an Ethylenically Unsaturated Bond] The first specific resin contains a group having an ethylenically unsaturated bond. The first specific resin may have the group having an ethylenically unsaturated bond in any part of the resin, but the group having an ethylenically unsaturated bond is preferably contained in the repeating unit represented by formula (1-1), and Y in the repeating unit represented by formula (1-1) 1 It is more preferable that the first specific resin is included in the above. Examples of the group having an ethylenically unsaturated bond include a group containing at least one group selected from the group consisting of a vinyl group, an allyl group, an isoallyl group, a 2-methylallyl group, a group having an aromatic ring directly bonded to a vinyl group (e.g., a vinylphenyl group), a (meth)acrylamide group, and a (meth)acryloyloxy group. In the present invention, "a direct bond between one structure and another structure" refers to a bond between one structure and another structure not via a linking group. From the viewpoint of reactivity, it is preferable that the first specific resin contains, as the group having an ethylenically unsaturated bond, a group having at least one group selected from the group consisting of a group having an aromatic ring directly bonded to a vinyl group, a (meth)acrylamide group, and a (meth)acryloyloxy group. From the viewpoint of reducing the dielectric dissipation factor, it is preferable that the first specific resin contains, as the group having an ethylenically unsaturated bond, a group having an aromatic ring directly bonded to a vinyl group, and more preferably a group having a vinylphenyl group.
[0022] The content of the group having an ethylenically unsaturated bond in the specific resin is preferably 0.1 to 3.0 mmol / g, more preferably 0.15 to 2.75 mmol / g, and even more preferably 0.2 to 2.5 mmol / g. Furthermore, when the specific resin contains a vinylphenyl group, the content of the vinylphenyl group in the specific resin is preferably 0.1 to 3.0 mmol / g, more preferably 0.15 to 2.75 mmol / g, and even more preferably 0.2 to 2.5 mmol / g.
[0023] [Repeating unit represented by formula (1-1)] The first specific resin contains a repeating unit represented by formula (1-1). The third specific resin preferably contains a repeating unit represented by formula (1-1). In this case, X in formula (1-1) 1 is a structure derived from a specific carboxylic acid compound described below, and Y 1 is a structure derived from the diamine compound of the present invention. In formula (1-1), X 1 represents a tetravalent organic group, Y 1 represents a divalent organic group.
[0024] -X 1 - In formula (1-1), X 1 Preferably, represents an organic group containing a structure obtained by removing two or more hydrogen atoms from a structure represented by any one of the following formulas (V-1) to (V-9), and more preferably represents an organic group containing a structure obtained by removing two or more hydrogen atoms from a structure represented by any one of formulas (V-1) to (V-4). By using an organic group containing a structure obtained by removing two or more hydrogen atoms from a structure represented by any one of formulas (V-1) to (V-9), the chemical resistance and flatness of the cured product are improved. Here, by using an organic group containing a structure obtained by removing two or more hydrogen atoms from a structure represented by any one of formulas (V-1) to (V-4), effects such as suppression of development residue generation, low dielectric constant of the cured product, and reduced thermal expansion coefficient are also obtained. Here, by using an organic group containing a structure obtained by removing two or more hydrogen atoms from a structure represented by any one of formulas (V-5) to (V-9), effects such as the cured product pattern being less likely to become tapered due to improved ultraviolet light transmittance and a wide tolerance for exposure dose are also obtained. In formula (V-2), R X1are each independently a hydrogen atom, an alkyl group, or a halogenated alkyl group. X2 and R X3 each independently represents a hydrogen atom or a substituent, R X2 and R X3 may bond to form a ring structure. X5 are each independently a hydrogen atom, an alkyl group, or a halogenated alkyl group.
[0025] In formula (V-2), R X1 are each independently preferably an alkyl group or a halogenated alkyl group, more preferably an alkyl group having 1 to 4 carbon atoms or a halogenated alkyl group having 1 to 4 carbon atoms, and even more preferably a methyl group or a trifluoromethyl group. A halogenated alkyl group refers to a group in which at least one hydrogen atom of an alkyl group has been substituted with a halogen atom. The halogen atom is preferably F or Cl, and more preferably F. In formula (V-3), R X2 and R X3 are each preferably independently a hydrogen atom. X2 and R X3 When R X2 and R X3 The structure formed by bonding is a single bond, —O— or —C(R) 2 - is preferred, and -O- or -C(R) 2 R represents a hydrogen atom or a monovalent organic group, preferably a hydrogen atom, an alkyl group, or an aryl group, more preferably a hydrogen atom. X5 are each independently preferably an alkyl group or a halogenated alkyl group, more preferably an alkyl group having 1 to 4 carbon atoms or a halogenated alkyl group having 1 to 4 carbon atoms, and even more preferably a methyl group or a trifluoromethyl group. A halogenated alkyl group refers to a group in which at least one hydrogen atom of an alkyl group has been substituted with a halogen atom. As the halogen atom, F or Cl is preferred, and F is more preferred.
[0026] X 1is a group containing a structure in which two or more hydrogen atoms have been removed from the structure represented by formula (V-1), X 1 is preferably a group represented by the following formula (V-1-1): 1 represents bonding sites with the four carbonyl groups to which n1 is bonded, and n1 represents an integer of 0 to 5, and is also preferably an integer of 1 to 5. Furthermore, the hydrogen atoms in the following structures may be further substituted with known substituents such as hydrocarbon groups.
[0027] X 1 is a group containing a structure in which two or more hydrogen atoms have been removed from the structure represented by formula (V-2), X 1 is preferably a group represented by the following formula (V-2-1) or formula (V-2-2), and from the viewpoint of lowering the amine value in the resin, it is preferably a group represented by formula (V-2-2). In this specification, a bond crossing a side of a ring structure means that it substitutes one of the hydrogen atoms in the ring structure. In the following formula, L X1 represents a single bond or —O—, and * represents X in formula (1-1). 1 represents the bonding site with the four carbonyl groups to which R is bonded. X1 The definitions and preferred embodiments of are as described above. In addition, the hydrogen atoms in these structures may be further substituted with known substituents such as hydrocarbon groups.
[0028] X 1 is a group containing a structure in which two or more hydrogen atoms have been removed from the structure represented by formula (V-3), X 1 is preferably a group represented by the following formula (V-3-1) or formula (V-3-2), and from the viewpoint of reducing the dielectric constant of the cured product, is preferably a group represented by formula (V-3-2). In the following formulas, * represents X in formula (1-1). 1 represents the bonding site with the four carbonyl groups to which R is bonded. X2 and R X3 The definitions and preferred embodiments of are as described above. In addition, the hydrogen atoms in these structures may be further substituted with known substituents such as hydrocarbon groups.
[0029] X 1 is a group containing a structure in which two or more hydrogen atoms have been removed from the structure represented by formula (V-4), X 1 is preferably a group represented by the following formula (V-4-1): In the following formula, * represents X in formula (1-1). 1 represents the bonding sites with the four carbonyl groups to which n is bonded, and n1 represents an integer of 0 to 5. In addition, the hydrogen atoms in the following structures may be further substituted with known substituents such as hydrocarbon groups. However, it is also preferred that none of the hydrogen atoms in the structure represented by (V-4-1) are substituted.
[0030] X 1 is a group containing a structure in which two or more hydrogen atoms have been removed from the structure represented by formula (V-5), X 1 is preferably a group represented by the following formula (V-5-1): In the following formula, * represents X in formula (1-1). 1 represents the bonding sites with the four carbonyl groups to which the carbonyl groups are bonded. In addition, the hydrogen atoms in the following structures may be further substituted with known substituents such as hydrocarbon groups.
[0031] X 1 is a group containing a structure in which two or more hydrogen atoms have been removed from the structure represented by formula (V-6), X 1 is preferably a group represented by the following formula (V-6-1): In the following formula, * represents X in formula (1-1). 1 represents the bonding sites with the four carbonyl groups to which the carbonyl groups are bonded. In addition, the hydrogen atoms in the following structures may be further substituted with known substituents such as hydrocarbon groups.
[0032] X 1 is a group containing a structure in which two or more hydrogen atoms have been removed from the structure represented by formula (V-7), X 1 is preferably a group represented by the following formula (V-7-1): In the following formula, * represents X in formula (1-1). 1 represents the bonding sites with the four carbonyl groups to which the carbonyl groups are bonded. In addition, the hydrogen atoms in the following structures may be further substituted with known substituents such as hydrocarbon groups.
[0033] X 1 is a group containing a structure in which two or more hydrogen atoms have been removed from the structure represented by formula (V-8), X 1 is preferably a group represented by the following formula (V-8-1): In the following formula, * represents X in formula (1-1). 1 represents the bonding sites with the four carbonyl groups to which the carbonyl groups are bonded. In addition, the hydrogen atoms in the following structures may be further substituted with known substituents such as hydrocarbon groups.
[0034] X 1 is a group containing a structure in which two or more hydrogen atoms have been removed from the structure represented by formula (V-9), X 1 is preferably a group represented by the following formula (V-9-1): In the following formula, * represents X in formula (1-1). 1 represents the bonding sites with the four carbonyl groups to which the carbonyl groups are bonded. In addition, the hydrogen atoms in the following structures may be further substituted with known substituents such as hydrocarbon groups.
[0035] Other, X 1 may be a tetracarboxylic acid residue remaining after removal of the anhydride group from a tetracarboxylic acid dianhydride described in paragraphs 0055 to 0057 of JP-A No. 2023-003421.
[0036] Also, X 1 It is preferable that X does not contain an imide bond in the structure. 1 In the present invention, the urethane bond is *—O—C(═O)—NR N - is a bond represented by *, and R N represents a hydrogen atom or a monovalent organic group, and * represents a bonding site with a carbon atom. N In the present invention, the urea bond is a bond represented by *-NR N —C(═O)—NR N - is a bond represented by *, and R NR each independently represents a hydrogen atom or a monovalent organic group, and * represents a bonding site with a carbon atom. N The preferred embodiments of X are as described above. 1 It is preferable that X does not contain an ester bond in its structure. In the present invention, the ester bond is a bond represented by *--O--C(=O)--*. Among these, X 1 It is preferable that the copolymer does not contain an imide bond, a urethane bond, a urea bond, or an amide bond, and it is more preferable that the copolymer does not contain an imide bond, a urethane bond, a urea bond, an amide bond, or an ester bond.
[0037] -Y 1 - In formula (1-1), Y 1 is preferably a group containing a group represented by formula (2-1), and more preferably a group represented by formula (2-1). In formula (2-1), R 1 and R 2 each independently represents a group having an ethylenically unsaturated bond, L represents a single bond or a divalent linking group not containing an imide bond, and * represents a bonding site to another structure.
[0038] In formula (2-1), R 1 and R 2 are each preferably independently a group represented by the following formula (R1-1): In formula (R1-1), L R1 represents an (n+1)-valent linking group, R R1 R each independently represents an aromatic group directly bonded to a vinyl group, a (meth)acryloxy group, or a (meth)acrylamide group, n represents an integer of 1 to 10, and * represents the bonding site with the oxygen atom in formula (2-1). R1 are each independently preferably an aromatic group directly bonded to a vinyl group, more preferably a vinylphenyl group. R1 is a hydrocarbon group, or a hydrocarbon group and —O—, —C(═O)—, —S—, —S(═O) 2 - and -NR N - is preferably a group represented by a bond to at least one group selected from the group consisting of a hydrocarbon group or * 1-C(=O)NR N -L R2 -* 2 The hydrocarbon group is preferably an alkylene group, more preferably an alkylene group having 1 to 10 carbon atoms, and even more preferably an alkylene group having 1 to 4 carbon atoms. N The preferred embodiments of the above are as described above. 1 has the same meaning as * in formula (R1-1), 2 is R in formula (R1-1) R1 represents the binding site with R R1 is a vinylphenyl group, L R1 is preferably an alkylene group having 1 to 4 carbon atoms, and more preferably a methylene group. R1 is a (meth)acryloxy group or a (meth)acrylamide group, L R1 teeth* 1 -C(=O)NR N -L R2 -* 2 n is preferably an integer of 1 to 4, more preferably 1 or 2, and even more preferably 1.
[0039] In formula (2-1), L is a single bond, —C(CH 3 ) 2 -, -C(CF 3 ) 2 -, -S(=O) 2 - or a 9,9-fluorenediyl group is preferred. 3 ) 2 -, or -C(CF 3 ) 2 The embodiment in which - is also one of the preferred embodiments of the present invention.
[0040] In addition, in formula (1-1), Y 1 may be a group containing a structure obtained by removing two or more hydrogen atoms from a structure represented by any one of the above formulas (V-1) to (V-9). By using an organic group containing a structure obtained by removing two or more hydrogen atoms from a structure represented by any one of formulas (V-1) to (V-9), the chemical resistance and flatness of the cured product are improved.
[0041] Y1 is a group containing a structure in which two or more hydrogen atoms have been removed from the structure represented by formula (V-1), Y 1 is preferably a group represented by the following formula (V-1-2): In the following formula, * represents Y in formula (1-1). 1 represents the bonding site to the two nitrogen atoms to which n is bonded, and n1 represents an integer of 1 to 5. Furthermore, the hydrogen atoms in the following structures may be further substituted with known substituents such as hydrocarbon groups.
[0042] Y 1 is a group containing a structure in which two or more hydrogen atoms have been removed from the structure represented by formula (V-2), 1 is preferably a group represented by the following formula (V-2-3) or formula (V-2-4), and from the viewpoint of reducing the dielectric constant of the cured product, it is preferably a group represented by formula (V-2-4). X1 represents a single bond or —O—, and * represents Y in formula (1-1). 1 represents the bonding site with the two nitrogen atoms to which R is bonded. X1 The preferred embodiments of are as described above. In addition, the hydrogen atoms in these structures may be further substituted with known substituents such as hydrocarbon groups.
[0043] Y 1 is a group containing a structure in which two or more hydrogen atoms have been removed from the structure represented by formula (V-3), 1 is preferably a group represented by the following formula (V-3-3) or formula (V-3-4), and from the viewpoint of reducing the dielectric constant of the cured product, it is preferably a group represented by formula (V-3-3). In the following formulas, * represents Y in formula (1-1). 1 represents the bonding site with the two nitrogen atoms to which the hydrogen atoms are bonded. In addition, the hydrogen atoms in these structures may be further substituted with known substituents such as hydrocarbon groups.
[0044] Y 1 is a group containing a structure in which two or more hydrogen atoms have been removed from the structure represented by formula (V-4), 1is preferably a group represented by the following formula (V-4-2): In the following formula, * represents Y in formula (1-1). 1 represents the bonding site to the two nitrogen atoms to which n is bonded, and n1 represents an integer of 0 to 5. An embodiment in which n1 is 0 is also one of the preferred embodiments of the present invention. Furthermore, the hydrogen atoms in the following structures may be further substituted with known substituents such as hydrocarbon groups.
[0045] Y 1 is a group containing a structure in which two or more hydrogen atoms have been removed from the structure represented by formula (V-5), 1 is preferably a group represented by the following formula (V-5-2): In the following formula, * represents Y in formula (1-1). 1 represents the bonding site with the two nitrogen atoms to which the hydrogen atoms are bonded. In addition, the hydrogen atoms in the following structures may be further substituted with known substituents such as hydrocarbon groups.
[0046] Y 1 is a group containing a structure in which two or more hydrogen atoms have been removed from the structure represented by formula (V-6), 1 is preferably a group represented by the following formula (V-6-2): In the following formula, * represents Y in formula (1-1). 1 represents the bonding site with the two nitrogen atoms to which the hydrogen atoms are bonded. In addition, the hydrogen atoms in the following structures may be further substituted with known substituents such as hydrocarbon groups.
[0047] Y 1 is a group containing a structure in which two or more hydrogen atoms have been removed from the structure represented by formula (V-7), 1 is preferably a group represented by the following formula (V-7-2): In the following formula, * represents Y in formula (1-1). 1 represents the bonding site with the two nitrogen atoms to which the hydrogen atoms are bonded. In addition, the hydrogen atoms in the following structures may be further substituted with known substituents such as hydrocarbon groups.
[0048] Y 1 is a group containing a structure in which two or more hydrogen atoms have been removed from the structure represented by formula (V-8), 1is preferably a group represented by the following formula (V-8-2): In the following formula, * represents Y in formula (1-1). 1 represents the bonding site with the two nitrogen atoms to which the carbon atoms are bonded. In addition, the hydrogen atoms in the following structures may be further substituted with known substituents such as hydrocarbon groups.
[0049] Y 1 is a group containing a structure in which two or more hydrogen atoms have been removed from the structure represented by formula (V-9), 1 is preferably a group represented by the following formula (V-9-2): In the following formula, * represents Y in formula (1-1). 1 represents the bonding site with the two nitrogen atoms to which the carbon atoms are bonded. In addition, the hydrogen atoms in the following structures may be further substituted with known substituents such as hydrocarbon groups.
[0050] Others, Y 1 may be a group described in paragraphs 0042 to 0053 of JP-A No. 2023-003421. 1 It is preferable that Y does not contain an imide bond in the structure. 1 It is preferable that Y does not contain a urethane bond, a urea bond, or an amide bond in the structure. 1 It is preferable that Y does not contain an ester bond in the structure. 1 It is preferable that the copolymer does not contain an imide bond, a urethane bond, a urea bond, or an amide bond, and it is more preferable that the copolymer does not contain an imide bond, a urethane bond, a urea bond, an amide bond, or an ester bond.
[0051] [Repeating unit represented by formula (1-2)] The first specific resin preferably contains a repeating unit represented by formula (1-2) below as the repeating unit represented by formula (1-1). The third specific resin preferably contains a repeating unit represented by formula (1-2). In this case, X in formula (1-2) 1 is a structure derived from a specific carboxylic acid compound described below, and Y 2 is a structure derived from the diamine compound of the present invention. In formula (1-2), X 1 represents a tetravalent organic group, Y2 represents a group containing a group represented by formula (2-1). 1 A preferred embodiment of the formula (1-1) is X 1 In formula (1-2), Y 2 A preferred embodiment of the group containing the group represented by formula (2-1) is Y in the above formula (1-1). 1 The preferred embodiments are the same as those of the group containing the group represented by formula (2-1) in the above.
[0052] [Repeating Unit Represented by Formula (1-3)] The second resin composition contains a repeating unit represented by the following formula (1-3). In formula (1-3), X 1 represents a tetravalent organic group, Y 3 represents a group containing a group represented by the following formula (2-2). In formula (2-2), R 1 and R 2 each independently represents a group having an ethylenically unsaturated bond, L represents a single bond, —C(CH 3 ) 2 -, or -C(CF 3 ) 2 - and * represent the binding site with other structures.
[0053] In formula (1-3), X 1 A preferred embodiment of the formula (1-1) is X 1 In formula (2-2), R 1 and R 2 A preferred embodiment of the formula (2-1) is R 1 and R 2 This is the same as the preferred embodiment of the above.
[0054] [Structures Represented by Formulae (3-1) to (3-3)] The specific resin preferably has a structure represented by any one of the following formulae (3-1) to (3-3). In formula (3-1), X 31 represents a tetravalent organic group, Y 31 represents a divalent organic group, R 31 represents a group having an ethylenically unsaturated bond, and * represents a bonding site with another structure. 31represents a tetravalent organic group, Y 31 represents a divalent organic group, R 31 represents a group having an ethylenically unsaturated bond, and * represents a bonding site with another structure. 31 represents a tetravalent organic group, Y 31 represents a divalent organic group, R 32 and R 33 each independently represents —OH or a monovalent organic group, and R 32 and R 33 At least one of the groups is a group having an ethylenically unsaturated bond, and * represents a bonding site to another structure.
[0055] In formulas (3-1) to (3-3), X 31 and Y 31 A preferred embodiment of the formula (1-1) is X 1 and Y 1 In formulas (3-1) to (3-3), R 31 ~R 33 Preferably, R contains a group having an ethylenically unsaturated bond, more preferably contains a group having an aromatic ring directly bonded to a vinyl group, and further preferably contains a group having a vinylphenyl group. 31 ~R 33 It is preferred that the formula does not contain an imide bond.
[0056] Among these, the specific resin preferably contains a structure represented by formula (3-1), and in formula (3-1), R 31 is preferably a group represented by the following formula (R3-1). In formula (R3-1), R 34 represents a substituent, n represents an integer of 0 to 5, and * represents the bonding site with the nitrogen atom in formula (3-1). 34 is preferably an alkyl group, an aryl group, or a group containing a group having an ethylenically unsaturated bond, and is preferably an alkyl group or a vinylphenylmethyl group. n is preferably 0 or 1, and more preferably 1.
[0057] [Reaction Product] The third specific resin is a reaction product of the diamine compound of the present invention and a compound having a total of two or more carboxy groups and carboxylic acid anhydride groups (also referred to as a "specific carboxylic acid compound") or a derivative thereof. Here, when the reaction to obtain the reaction product is carried out by chemical imidization, the third specific resin is preferably a reaction product of the diamine compound of the present invention and a specific carboxylic acid compound. The first specific resin and the second specific resin are preferably reaction products of the diamine compound of the present invention and a compound having two carboxylic acid anhydride groups or a derivative thereof. Details of the diamine compound of the present invention will be described later.
[0058] The diamine compound of the present invention contains a group having an ethylenically unsaturated bond, as described later. Here, when it is desired to introduce a group represented by the above formula (2-1) into a specific resin, for example, a structure having a phenolic hydroxyl group as represented by the following formula (2-1C) can be introduced into the Y 1 and then reacting the phenolic hydroxyl group with a compound that contains a group having an ethylenically unsaturated bond and that reacts with a phenolic hydroxyl group, such as an isocyanate compound containing a group having an ethylenically unsaturated bond, to form R 1 , R 2 It is also possible to form In formula (2-C), L has the same meaning as L in formula (2-1) above, and preferred embodiments are also similar. However, according to such an embodiment, phenolic hydroxyl groups may remain in the resin, resulting in variations in the amount of groups having ethylenically unsaturated bonds introduced. Such variations in the amount introduced may result in variations in the elongation at break of the cured film, and the residual phenolic hydroxyl groups may increase the dielectric dissipation factor of the cured film. Because the diamine of the present invention contains a group having an ethylenically unsaturated bond, using this in a reaction with a specific carboxylic acid compound facilitates the introduction of the group represented by formula (2-1) into the resin, thereby preventing residual phenolic hydroxyl groups from remaining in the resin. As a result, it is believed that the effects of suppressing variations in the elongation at break of the cured product and reducing the dielectric dissipation factor are achieved.
[0059] Examples of the specific carboxylic acid compound include a compound having two carboxy groups, a compound having one carboxy group and one carboxylic acid anhydride group, and a compound having two carboxylic acid anhydride groups, and a compound having two carboxylic acid anhydride groups (i.e., a carboxylic acid dianhydride) is preferred.
[0060] By using a compound having two carboxylic acid anhydride groups or a derivative thereof, a specific resin that is a polyimide can be obtained. Examples of derivatives of compounds having two carboxylic acid anhydride groups include diesters of compounds having two carboxylic acid anhydride groups, and diester dihalide compounds obtained from compounds having two carboxylic acid anhydride groups. The diesters can be obtained, for example, by reacting a compound having two carboxylic acid anhydride groups with an alkylating agent or an alcohol. Examples of the alkylating agent include N,N-dimethylformamide dimethyl acetal, N,N-dimethylformamide diethyl acetal, N,N-dialkylformamide dialkyl acetal, trimethyl orthoformate, and triethyl orthoformate. Examples of the alcohols include R C1 Examples of compounds represented by —OH include R C1 represents R in formula (C1-2) described below. C1 The same applies to the preferred embodiments. The diester dihalide compound can be obtained, for example, by reacting the diester with a halogenating agent. Examples of the halogenating agent include thionyl chloride, oxalyl chloride, and phosphorus oxychloride.
[0061] Examples of compounds having two carboxylic acid anhydride groups or derivatives thereof include, but are not limited to, compounds represented by the following formulas (C1-1) to (C1-3). When the reaction to obtain the reaction product is carried out by chemical imidization, the compound represented by formula (C1-1) is preferred. In formula (C1-1), X 1 represents a tetravalent organic group. 1 represents a tetravalent organic group, R C1Each of X independently represents a monovalent organic group. 1 represents a tetravalent organic group, R C1 Each of X independently represents a monovalent organic group. 1 A preferred embodiment of the formula (1-1) is X 1 In formula (C1-2) to formula (C1-3), R C1 A preferred embodiment of the present invention is R 113 and R 114 This is the same as the preferred embodiment of the above.
[0062] By using a compound having one carboxy group and one carboxylic anhydride group, a specific resin that is a polyamideimide can be obtained.
[0063] By using a compound having two carboxylic acid anhydride groups, a specific resin that is a polyamide can be obtained.
[0064] [Details of the Reaction to Obtain a Reaction Product] In the reaction to obtain a reaction product, it is preferable to use an organic solvent during the reaction. One or more organic solvents may be used. The organic solvent can be appropriately selected depending on the raw materials, and examples thereof include pyridine, diethylene glycol dimethyl ether (diglyme), N-methylpyrrolidone, N-ethylpyrrolidone, ethyl propionate, dimethylacetamide, dimethylformamide, tetrahydrofuran, and γ-butyrolactone. In the reaction to obtain a reaction product, it is preferable to add a basic compound during the reaction. One or more basic compounds may be used. The basic compound can be appropriately selected depending on the raw materials, and examples thereof include triethylamine, diisopropylethylamine, pyridine, 1,8-diazabicyclo[5.4.0]undec-7-ene, and N,N-dimethyl-4-aminopyridine. Furthermore, when the reaction product is a compound having an imide bond, imidization can be promoted (chemical imidization) by using a dehydration cycloreductant, such as a combination of a carboxylic acid anhydride and an amine, in the reaction to obtain the reaction product. Examples of the dehydration cycloreductant include reagents known in the field of chemical imidization, such as a combination of acetic anhydride and pyridine. Chemical imidization allows the imidization reaction to proceed at low temperatures and reduces the likelihood of remaining open rings. This has the advantages of suppressing oxidative discoloration of the amine, reducing the likelihood of remaining open rings, thereby reducing the likelihood of remaining carboxyl or amide groups, improving the reliability of the cured product, and reducing the dielectric loss tangent. Furthermore, since the diamine compound of the present invention contains a group having an ethylenically unsaturated bond, it is preferable to add a polymerization inhibitor to the reaction to obtain the reaction product. Examples of polymerization inhibitors include the polymerization inhibitors contained in the resin composition of the present invention described below.
[0065] It is also preferable to use an end-capping agent in the reaction to obtain the reaction product. Examples of end-capping agents include monoalcohols, phenols, thiols, thiophenols, monoamines, etc., and from the perspective of reactivity and film stability, it is more preferable to use monoalcohols, phenols, or monoamines. Preferred monoalcohol compounds include primary alcohols such as methanol, ethanol, propanol, butanol, hexanol, octanol, dodecynol, benzyl alcohol, 2-phenylethanol, 2-methoxyethanol, 2-chloromethanol, and furfuryl alcohol; secondary alcohols such as isopropanol, 2-butanol, cyclohexyl alcohol, cyclopentanol, and 1-methoxy-2-propanol; and tertiary alcohols such as t-butyl alcohol and adamantane alcohol. Preferred phenol compounds include phenols such as phenol, methoxyphenol, methylphenol, naphthalene-1-ol, naphthalene-2-ol, and hydroxystyrene. Preferred examples of the monoamine compound include aniline, 2-ethynylaniline, 3-ethynylaniline, 4-ethynylaniline, 5-amino-8-hydroxyquinoline, 1-hydroxy-7-aminonaphthalene, 1-hydroxy-6-aminonaphthalene, 1-hydroxy-5-aminonaphthalene, 1-hydroxy-4-aminonaphthalene, 2-hydroxy-7-aminonaphthalene, 2-hydroxy-6-aminonaphthalene, 2-hydroxy-5-aminonaphthalene, 1-carboxy-7-aminonaphthalene, 1-carboxy-6-aminonaphthalene, 1-carboxy-5-aminonaphthalene, Examples of the aminobenzoic acid include 2-carboxy-7-aminonaphthalene, 2-carboxy-6-aminonaphthalene, 2-carboxy-5-aminonaphthalene, 2-aminobenzoic acid, 3-aminobenzoic acid, 4-aminobenzoic acid, 4-aminosalicylic acid, 5-aminosalicylic acid, 6-aminosalicylic acid, 2-aminobenzenesulfonic acid, 3-aminobenzenesulfonic acid, 4-aminobenzenesulfonic acid, 3-amino-4,6-dihydroxypyrimidine, 2-aminophenol, 3-aminophenol, 4-aminophenol, 2-aminothiophenol, 3-aminothiophenol, and 4-aminothiophenol.Two or more of these may be used, or multiple different end groups may be introduced by reacting multiple end-capping agents. Furthermore, when capping the amino groups at the resin terminals, they can be capped with a compound having a functional group capable of reacting with the amino group. Preferred capping agents for amino groups include carboxylic acid anhydrides, carboxylic acid chlorides, carboxylic acid bromides, sulfonic acid chlorides, sulfonic acid anhydrides, and sulfonic acid carboxylic acid anhydrides, with carboxylic acid anhydrides and carboxylic acid chlorides being more preferred. Preferred carboxylic acid anhydride compounds include acetic anhydride, propionic acid anhydride, oxalic acid anhydride, succinic acid anhydride, maleic acid anhydride, phthalic acid anhydride, benzoic acid anhydride, and 5-norbornene-2,3-dicarboxylic acid anhydride. Furthermore, preferred carboxylic acid chloride compounds include acetyl chloride, acrylic acid chloride, propionyl chloride, methacrylic acid chloride, pivaloyl chloride, cyclohexanecarbonyl chloride, 2-ethylhexanoyl chloride, cinnamoyl chloride, 1-adamantanecarbonyl chloride, heptafluorobutyryl chloride, stearic acid chloride, and benzoyl chloride. Furthermore, by using an end-capping agent containing a group having an ethylenically unsaturated bond, it is also possible to introduce a structure represented by any one of the above formulas (3-1) to (3-3) into a specific resin. For example, by using a monoamine represented by the following formula (AM-1), a structure represented by formula (3-1), in which R 31 It is possible to introduce a structure in which is a group represented by (R3-1).
[0066] The reaction temperature in the reaction to obtain the reaction product is preferably 150 to 350° C., and more preferably 160 to 250° C., when thermal imidization is performed. However, as described above, in the present invention, it is also preferable to perform the reaction at a low temperature by chemical imidization, and in that case, the reaction temperature is preferably room temperature (23° C.) to 100° C., and more preferably 50 to 90° C. The reaction temperature may be determined by referring to known conditions or by taking into consideration the rate of change of the imide group value, which will be described later, and the like.
[0067] The reaction time in the reaction to obtain the reaction product (i.e., the time for exposure to the reaction temperature) is not particularly limited and may be determined by referring to known conditions or by taking into consideration the rate of change of the imide group value, which will be described later, and the like. For example, the reaction time may be 30 minutes to 24 hours, preferably 1 to 15 hours, more preferably 2 to 10 hours, and even more preferably 3 to 8 hours.
[0068] After the reaction to obtain the reaction product, a step of precipitating a solid may be included. Specifically, after filtering out the water-absorbing by-product of the dehydration condensation agent coexisting in the reaction solution as needed, the obtained polymer component is added to a poor solvent such as water, aliphatic lower alcohol, or a mixture thereof to precipitate the polymer component as a solid, and then dried to obtain a specific resin such as polyimide. To improve the degree of purification, the specific resin such as polyimide may be repeatedly subjected to operations such as redissolution, reprecipitation, and drying. Furthermore, a step of removing ionic impurities using an ion exchange resin may be included.
[0069] The specific resin is preferably a resin whose rate of change in imide group value before and after heating at 350°C under 1 atmosphere for 1 hour is 25% or less, as calculated by the following formula: Rate of change (%) = (Im2 - Im1) x 100 / Im1, where Im1 is the imide group value (mmol / g) before heating and Im2 is the imide group value (mmol / g) after heating at 350°C under 1 atmosphere for 1 hour.
[0070] The rate of change is preferably 15% or less, and more preferably 10% or less. There is no particular lower limit to the rate of change, as long as it is 0% or more.
[0071] The rate of change is measured, for example, by the following method: measuring the infrared absorption spectrum of a specific resin, and detecting the absorption peak at 1377 cm -1 Next, the specific resin is heat-treated at 350°C and 1 atmosphere for 1 hour, and then the infrared absorption spectrum is measured again to determine the peak intensity P1 around 1377 cm -1The peak intensity P2 around the peak intensity P1 is then measured. Using the obtained peak intensities P1 and P2, the rate of change in the imide value can be calculated based on the following formula: Peak intensity P1 is an index showing the imide value Im1 before heating, and peak intensity P2 is an index showing the imide value Im2 after heating. Rate of change in imide value (%) = (peak intensity P2 - peak intensity P1) x 100 / peak intensity P1
[0072] The content of the repeating unit represented by formula (1-1) relative to the total mass of the specific resin is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more. The upper limit of the content is not particularly limited and may be 100% by mass. Furthermore, the specific resin may contain two or more types of repeating units represented by formula (1-1). In that case, it is preferable that the total amount is within the above range.
[0073] The content of the repeating unit represented by formula (1-2) relative to the total mass of the specific resin is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 40% by mass or more. The upper limit of this content is not particularly limited and may be 100% by mass. Furthermore, the specific resin may contain two or more types of repeating units represented by formula (1-2). In this case, it is preferable that the total amount is within the above range.
[0074] The content of the repeating unit represented by formula (1-3) relative to the total mass of the specific resin is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 40% by mass or more. The upper limit of this content is not particularly limited and may be 100% by mass. Furthermore, the specific resin may contain two or more types of repeating units represented by formula (1-1). In that case, it is preferable that the total amount is within the above range.
[0075] The weight-average molecular weight (Mw) of the specific resin is preferably 3,000 to 100,000. The lower limit of the Mw is preferably 5,000 or more, more preferably 8,000 or more, and even more preferably 10,000 or more. The upper limit of the Mw is preferably 50,000 or less, more preferably 40,000 or less, and even more preferably 25,000 or less. By setting the weight-average molecular weight to 3,000 or more, the fold resistance of the cured film can be improved. In order to obtain an organic film with excellent mechanical properties (e.g., breaking elongation), the weight-average molecular weight is particularly preferably 5,000 or more. The number-average molecular weight (Mn) of the specific resin is preferably 1,000 to 40,000, more preferably 2,000 to 30,000, even more preferably 5,000 to 20,000, and particularly preferably 6,000 to 12,000. The molecular weight dispersity of the specific resin is preferably 1.5 or more, more preferably 1.8 or more, and even more preferably 2.0 or more. In this specification, the molecular weight dispersity is a value calculated by weight average molecular weight / number average molecular weight. The upper limit of the molecular weight dispersity of the specific resin is not particularly specified, but for example, it is preferably 7.0 or less, more preferably 6.5 or less, even more preferably 6.0 or less, even more preferably 4.5 or less, and particularly preferably 3.0 or less. When the resin composition contains multiple specific resins as specific resins, it is preferable that the weight average molecular weight, number average molecular weight, and dispersity of at least one specific resin are within the above ranges. It is also preferable that the weight average molecular weight, number average molecular weight, and dispersity calculated by treating the multiple specific resins as one resin are each within the above ranges.
[0076] [Specific Examples] Specific examples of the specific resin include polyimides (A-1) to (A-20) in the examples described below, but the present invention is not limited to these.
[0077] [Content] The content of the specific resin in the resin composition of the present invention is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, even more preferably 50% by mass or more, and most preferably 60% by mass or more, based on the total solid content of the resin composition. Furthermore, the content of the resin in the resin composition of the present invention is preferably 99.5% by mass or less, more preferably 99% by mass or less, even more preferably 98% by mass or less, even more preferably 97% by mass or less, and even more preferably 95% by mass or less, based on the total solid content of the resin composition. The resin composition of the present invention may contain only one type of specific resin, or may contain two or more types. When two or more types are contained, the total amount is preferably within the above range.
[0078] <Other Resins> The resin composition of the present invention may contain the specific resin described above and other resins different from the specific resin (hereinafter simply referred to as "other resins"). Examples of other resins include resins different from the specific resin, such as polyimide precursors, polyimides, polybenzoxazole precursors, polybenzoxazoles, polyamideimide precursors, polyamideimides, aromatic polyethers, phenolic resins, polyamides, epoxy resins, polysiloxanes, resins containing a siloxane structure, (meth)acrylic resins, (meth)acrylamide resins, urethane resins, butyral resins, styryl resins, polyether resins, and polyester resins. Examples of other polyimide precursors, other polyimides, polybenzoxazole precursors, polybenzoxazoles, polyamideimide precursors, and polyamideimides include the compounds described in paragraphs 0017 to 0138 of WO 2022 / 145355. The above descriptions are incorporated herein by reference.
[0079] The aromatic polyether is not particularly limited, but is preferably polyphenylene ether. The polyphenylene ether preferably contains a repeating unit represented by the following formula (PE): In formula (PE), R E1represents a hydrogen atom or a substituent. Examples of the substituent include a halogen atom, an alkyl group which may have a substituent, an alkoxy group which may have a substituent, an amino group which may have a substituent, a nitro group, and a carboxy group.
[0080] Furthermore, the polyphenylene ether is preferably a compound having a polymerizable group. The polymerizable group is preferably an epoxy group, an oxetanyl group, an oxazolyl group, a methylol group, an alkoxymethyl group, an acyloxymethyl group, a blocked isocyanate group, or a group having an ethylenically unsaturated bond, with a group having an ethylenically unsaturated bond being more preferred. Examples of the group having an ethylenically unsaturated bond include a vinyl group, an allyl group, an isoallyl group, a 2-methylallyl group, a group having an aromatic ring directly bonded to a vinyl group (e.g., a vinylphenyl group), a (meth)acrylamide group, and a (meth)acryloyloxy group. A vinylphenyl group, a (meth)acrylamide group, or a (meth)acryloyloxy group is preferred, a vinylphenyl group or a (meth)acryloyloxy group is more preferred, and a (meth)acryloyloxy group is even more preferred. When the polyphenylene ether is a compound having a polymerizable group, the position of the polymerizable group is not particularly limited, but for example, a structure in which the polymerizable group is introduced at the end of the main chain is preferred.
[0081] The polyphenylene ether may contain other repeating units, provided that the content of the other repeating units is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 10% by mass or less, based on the total mass of the polyphenylene ether.
[0082] The number average molecular weight of the polyphenylene ether is not particularly limited, but is preferably 500 to 50,000. The lower limit of the number average molecular weight is preferably 800 or more, more preferably 1,000 or more, and even more preferably 1,500 or more. The upper limit of the number average molecular weight is preferably 30,000 or less, more preferably 20,000 or less, and even more preferably 10,000 or less.
[0083] Specific examples of polyphenylene ether (PPE) include, but are not limited to, poly(2,6-dimethyl-1,4-phenylene ether), poly(2-methyl-6-ethyl-1,4-phenylene ether), poly(2-methyl-6-phenyl-1,4-phenylene ether), poly(2,6-dichloro-1,4-phenylene ether), copolymers of 2,6-dimethylphenol and other phenols (e.g., 2,3,6-trimethylphenol, 2-methyl-6-butylphenol, etc.), polyphenylene ether copolymers obtained by coupling 2,6-dimethylphenol with biphenols or bisphenols, and polyphenylene ethers having a linear or branched structure obtained by heating poly(2,6-dimethyl-1,4-phenylene ether) or the like with a phenolic compound such as a bisphenol or trisphenol in a toluene solvent in the presence of an organic peroxide to cause a redistribution reaction.
[0084] When the resin composition of the present invention contains another resin, the content of the other resin is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, even more preferably 1% by mass or more, even more preferably 2% by mass or more, even more preferably 5% by mass or more, and even more preferably 10% by mass or more, based on the total solid content of the resin composition. The content of the other resin in the resin composition of the present invention is preferably 80% by mass or less, more preferably 75% by mass or less, even more preferably 70% by mass or less, even more preferably 60% by mass or less, and even more preferably 50% by mass or less, based on the total solid content of the resin composition. A preferred embodiment of the resin composition of the present invention may also be an embodiment in which the content of the other resin is low. In the above embodiment, the content of the other resin is preferably 20% by mass or less, more preferably 15% by mass or less, even more preferably 10% by mass or less, even more preferably 5% by mass or less, and even more preferably 1% by mass or less, based on the total solid content of the resin composition. The lower limit of the content is not particularly limited, as long as it is 0% by mass or more. Furthermore, when the resin composition of the present invention contains other resins, the content of the specific resin relative to the total content of the specific resin and the other resins is preferably 40 to 90 mass%, more preferably 50 to 80 mass%, and even more preferably 55 to 70 mass%. The resin composition of the present invention may contain only one type of other resin, or may contain two or more types. When two or more types are contained, it is preferable that the total amount is in the above range.
[0085] <Polymerizable Compound Having an Ethylenically Unsaturated Bond> The resin composition of the present invention contains a polymerizable compound having an ethylenically unsaturated bond. The polymerizable compound having an ethylenically unsaturated bond has a group containing an ethylenically unsaturated bond. Examples of the group containing an ethylenically unsaturated bond include a vinyl group, an allyl group, a vinylphenyl group, a (meth)acryloyl group, a maleimide group, and a (meth)acrylamide group. Among these, a (meth)acryloyl group, a (meth)acrylamide group, and a vinylphenyl group are preferred, and from the viewpoint of reactivity, a (meth)acryloyl group is more preferred.
[0086] The polymerizable compound having an ethylenically unsaturated bond is preferably a compound having one or more groups containing an ethylenically unsaturated bond, more preferably a compound having two or more groups containing an ethylenically unsaturated bond. The polymerizable compound having an ethylenically unsaturated bond may have three or more groups containing an ethylenically unsaturated bond. The compound having two or more groups containing an ethylenically unsaturated bond is preferably a compound having 2 to 15 groups containing an ethylenically unsaturated bond, more preferably a compound having 2 to 10 groups, and even more preferably a compound having 2 to 6 groups. From the viewpoint of the film strength of the obtained pattern (cured product), it is also preferable that the resin composition of the present invention contains a compound having two groups containing an ethylenically unsaturated bond and a compound having three or more groups containing an ethylenically unsaturated bond.
[0087] The molecular weight of the polymerizable compound having an ethylenically unsaturated bond is preferably 2,000 or less, more preferably 1,500 or less, and even more preferably 900 or less. The lower limit of the molecular weight of the polymerizable compound having an ethylenically unsaturated bond is preferably 100 or more.
[0088] Specific examples of polymerizable compounds having an ethylenically unsaturated bond include unsaturated carboxylic acids (e.g., acrylic acid, methacrylic acid, itaconic acid, crotonic acid, isocrotonic acid, maleic acid, etc.) and their esters and amides. Preferred are esters of unsaturated carboxylic acids and polyhydric alcohols, and amides of unsaturated carboxylic acids and polyamines. Also suitable are addition reaction products of unsaturated carboxylic acid esters or amides having a nucleophilic substituent, such as a hydroxyl group, an amino group, or a sulfanyl group, with monofunctional or polyfunctional isocyanates or epoxies, and dehydration condensation reaction products of monofunctional or polyfunctional carboxylic acids. Also suitable are addition reaction products of unsaturated carboxylic acid esters or amides having an electrophilic substituent, such as an isocyanate group or an epoxy group, with monofunctional or polyfunctional alcohols, amines, or thiols, and substitution reaction products of unsaturated carboxylic acid esters or amides having a leaving substituent, such as a halogeno group or a tosyloxy group, with monofunctional or polyfunctional alcohols, amines, or thiols. As another example, it is also possible to use a group of compounds in which the above-mentioned unsaturated carboxylic acids are replaced with unsaturated phosphonic acids, vinylbenzene derivatives such as styrene, vinyl ethers, allyl ethers, etc. Specific examples can be found in paragraphs 0113 to 0122 of JP 2016-027357 A, the contents of which are incorporated herein by reference.
[0089] The polymerizable compound having an ethylenically unsaturated bond is preferably a compound having a boiling point of 100°C or higher under normal pressure. Examples of compounds having a boiling point of 100°C or higher under normal pressure include the compounds described in paragraph 0203 of WO 2021 / 112189. The contents of this specification are incorporated herein by reference.
[0090] Other preferred polymerizable compounds having an ethylenically unsaturated bond than those described above include the radical polymerizable compounds described in paragraphs 0204 to 0208 of WO 2021 / 112189, the contents of which are incorporated herein by reference.
[0091] Preferred polymerizable compounds having an ethylenically unsaturated bond include dipentaerythritol triacrylate (commercially available products include KAYARAD D-330 (manufactured by Nippon Kayaku Co., Ltd.)), dipentaerythritol tetraacrylate (commercially available products include KAYARAD D-320 (manufactured by Nippon Kayaku Co., Ltd.) and A-TMMT (manufactured by Shin-Nakamura Chemical Co., Ltd.)), dipentaerythritol penta(meth)acrylate (commercially available products include KAYARAD D-310 (manufactured by Nippon Kayaku Co., Ltd.)), and dipentaerythritol hexa(meth)acrylate (commercially available products include KAYARAD DPHA (manufactured by Nippon Kayaku Co., Ltd.) and A-DPH (manufactured by Shin-Nakamura Chemical Co., Ltd.)), and structures in which the (meth)acryloyl group is bonded via an ethylene glycol residue or a propylene glycol residue. Oligomer types of these compounds can also be used.
[0092] Commercially available polymerizable compounds having an ethylenically unsaturated bond include, for example, SR-494, a tetrafunctional acrylate having four ethyleneoxy chains, SR-209, 231, and 239, which are difunctional methacrylates having four ethyleneoxy chains (all manufactured by Sartomer Corporation), DPCA-60, a hexafunctional acrylate having six pentyleneoxy chains, and TPA-330, a trifunctional acrylate having three isobutyleneoxy chains (all manufactured by Nippon Kayaku Co., Ltd.), and urethane Examples of such an acrylic acid copolymer include acrylic acid copolymers UAS-10 and UAB-140 (manufactured by Nippon Paper Industries Co., Ltd.), NK Ester M-40G, NK Ester 4G, NK Ester M-9300, NK Ester A-9300, and UA-7200 (manufactured by Shin-Nakamura Chemical Co., Ltd.), DPHA-40H (manufactured by Nippon Kayaku Co., Ltd.), UA-306H, UA-306T, UA-306I, AH-600, T-600, and AI-600 (manufactured by Kyoeisha Chemical Co., Ltd.), and Blenmar PME400 (manufactured by NOF Corporation).
[0093] Suitable polymerizable compounds having an ethylenically unsaturated bond include urethane acrylates such as those described in JP-B No. 48-041708, JP-A No. 51-037193, JP-B No. 02-032293, and JP-B No. 02-016765, and urethane compounds having an ethylene oxide skeleton such as those described in JP-B No. 58-049860, JP-B No. 56-017654, JP-B No. 62-039417, and JP-B No. 62-039418. Suitable polymerizable compounds having an ethylenically unsaturated bond include compounds having an amino structure or a sulfide structure in the molecule, as described in JP-A No. 63-277653, JP-A No. 63-260909, and JP-A No. 01-105238.
[0094] The polymerizable compound having an ethylenically unsaturated bond may be a compound having an acid group such as a carboxy group or a phosphate group. The polymerizable compound having an ethylenically unsaturated bond and an acid group is preferably an ester of an aliphatic polyhydroxy compound and an unsaturated carboxylic acid, and more preferably a polymerizable compound having an ethylenically unsaturated bond in which an acid group is provided by reacting an unreacted hydroxy group of an aliphatic polyhydroxy compound with a non-aromatic carboxylic acid anhydride. Particularly preferred are polymerizable compounds having an ethylenically unsaturated bond in which an acid group is provided by reacting an unreacted hydroxy group of an aliphatic polyhydroxy compound with a non-aromatic carboxylic acid anhydride, in which the aliphatic polyhydroxy compound is pentaerythritol or dipentaerythritol. Examples of commercially available products include polybasic acid-modified acrylic oligomers M-510 and M-520 manufactured by Toagosei Co., Ltd.
[0095] The acid value of the polymerizable compound having an ethylenically unsaturated bond with an acid group is preferably 0.1 to 300 mgKOH / g, more preferably 1 to 100 mgKOH / g. When the acid value of the polymerizable compound having an ethylenically unsaturated bond is within the above range, the compound has excellent handleability in production and developability. In addition, the compound has good polymerizability. The acid value is measured in accordance with the description of JIS K 0070:1992.
[0096] As the polymerizable compound having an ethylenically unsaturated bond, a polymerizable compound having an ethylenically unsaturated bond with at least one selected from the group consisting of a urea bond and a urethane bond (hereinafter also referred to as "polymerizable compound U"). In the present invention, the urea bond is a bond represented by the following formula: *-NR N —C(═O)—NR N - is a bond represented by *, and R N Each of the *'s independently represents a hydrogen atom or a monovalent organic group, and each * represents a bonding site with a carbon atom. In the present invention, the urethane bond is *—O—C(═O)—NR N - is a bond represented by *, and R N represents a hydrogen atom or a monovalent organic group, and * represents a bonding site with a carbon atom. The inclusion of polymerizable compound U in a resin composition may improve chemical resistance, resolution, and the like. While the mechanism by which this effect is achieved is unclear, it is thought that, for example, upon curing by heating, a portion of polymerizable compound U is thermally decomposed to generate amines, which then promote the cyclization of precursors of cyclized resins, such as polyimide precursors. Polymerizable compound U may have only one urea bond or urethane bond, one or more urea bonds and one or more urethane bonds, no urethane bonds but two or more urea bonds, or no urea bonds but two or more urethane bonds. The total number of urea bonds and urethane bonds in polymerizable compound U is 1 or more, preferably 1 to 10, more preferably 1 to 4, and even more preferably 1 or 2. When polymerizable compound U does not have a urethane bond, the number of urea bonds in polymerizable compound U is 1 or more, preferably 1 to 10, more preferably 1 to 4, and even more preferably 1 or 2. When the polymerizable compound U does not have a urea bond, the number of urethane bonds in the polymerizable compound U is 1 or more, preferably 1 to 10, more preferably 1 to 4, and even more preferably 1 or 2.
[0097] The radical polymerizable group in the polymerizable compound U is not particularly limited, but examples thereof include a vinyl group, an allyl group, a (meth)acryloyl group, a (meth)acryloxy group, a (meth)acrylamide group, a vinylphenyl group, and a maleimide group. A (meth)acryloxy group, a (meth)acrylamide group, a vinylphenyl group, or a maleimide group is preferred, and a (meth)acryloxy group is more preferred. When the polymerizable compound U has two or more radical polymerizable groups, the structures of the respective radical polymerizable groups may be the same or different. The number of radical polymerizable groups in the polymerizable compound U may be only one or may be two or more, preferably 1 to 10, more preferably 1 to 6, and particularly preferably 1 to 4. The radical polymerizable group value (mass of the compound per mole of radical polymerizable group) in the polymerizable compound U is preferably 150 to 400 g / mol. From the viewpoint of chemical resistance of the cured product, the lower limit of the radical polymerizable group value is more preferably 200 g / mol or more, even more preferably 210 g / mol or more, even more preferably 220 g / mol or more, even more preferably 230 g / mol or more, still more preferably 240 g / mol or more, and particularly preferably 250 g / mol or more. From the viewpoint of developability, the upper limit of the radical polymerizable group value is more preferably 350 g / mol or less, even more preferably 330 g / mol or less, and particularly preferably 300 g / mol or less. In particular, the polymerizable group value of polymerizable compound U is preferably 210 to 400 g / mol, and more preferably 220 to 400 g / mol.
[0098] The polymerizable compound U preferably has a structure represented by the following formula (U-1), for example. In formula (U-1), R U1 represents a hydrogen atom or a monovalent organic group, and A represents —O— or —NR N - and R N is a hydrogen atom or a monovalent organic group, Z U1 is an m-valent organic group, and Z U2 is an (n+1)-valent organic group, X is a radical polymerizable group, n is an integer of 1 or more, and m is an integer of 1 or more.
[0099] R U1 R is preferably a hydrogen atom, an alkyl group or an aromatic hydrocarbon group, and more preferably a hydrogen atom. N is preferably a hydrogen atom, an alkyl group or an aromatic hydrocarbon group, more preferably a hydrogen atom. U1 represents a hydrocarbon group, -O-, -C(=O)-, -S-, -S(=O) 2 -, -NR N - or a group in which two or more of these are bonded is preferred, and a hydrocarbon group, or a hydrocarbon group and -O-, -C(=O)-, -S-, -S(=O) 2 - and -NR N - is more preferred. The hydrocarbon group is preferably a hydrocarbon group having 20 or less carbon atoms, more preferably a hydrocarbon group having 18 or less carbon atoms, and even more preferably a hydrocarbon group having 16 or less carbon atoms. Examples of the hydrocarbon group include saturated aliphatic hydrocarbon groups, aromatic hydrocarbon groups, and groups represented by a combination of these. R N represents a hydrogen atom or a monovalent organic group, preferably a hydrogen atom or a hydrocarbon group, more preferably a hydrogen atom or an alkyl group, and even more preferably a hydrogen atom or a methyl group. U2 represents a hydrocarbon group, -O-, -C(=O)-, -S-, -S(=O) 2 -, -NR N - or a group in which two or more of these are bonded is preferred, and a hydrocarbon group, or a hydrocarbon group and -O-, -C(=O)-, -S-, -S(=O) 2 - and -NR N A group bonded to at least one group selected from the group consisting of - is more preferred. U1Examples of the groups include those listed in 1. and preferred embodiments are also the same. X is not particularly limited, but examples include a vinyl group, an allyl group, a (meth)acryloyl group, a (meth)acryloxy group, a (meth)acrylamide group, a vinylphenyl group, and a maleimide group, with a (meth)acryloxy group, a (meth)acrylamide group, a vinylphenyl group, or a maleimide group being preferred, and a (meth)acryloxy group being more preferred. n is preferably an integer of 1 to 10, more preferably an integer of 1 to 4, even more preferably 1 or 2, and particularly preferably 1. m is preferably an integer of 1 to 10, more preferably an integer of 1 to 4, and even more preferably 1 or 2.
[0100] It is also preferable that the polymerizable compound U has at least one of a hydroxy group, an alkyleneoxy group, an amide group, and a cyano group. From the viewpoint of the chemical resistance of the resulting cured film, the hydroxy group may be an alcoholic hydroxy group or a phenolic hydroxy group, but is preferably an alcoholic hydroxy group. From the viewpoint of the chemical resistance of the resulting cured film, the alkyleneoxy group is preferably an alkyleneoxy group having 2 to 20 carbon atoms, more preferably an alkyleneoxy group having 2 to 10 carbon atoms, even more preferably an alkyleneoxy group having 2 to 4 carbon atoms, even more preferably an ethylene group or a propylene group, and particularly preferably an ethylene group. The alkyleneoxy group may be contained in the polymerizable compound U as a polyalkyleneoxy group. In this case, the number of repeating units of the alkyleneoxy group is preferably 2 to 10, more preferably 2 to 6. The amide group is represented by -C(=O)-NR N - refers to a bond represented by R N When the polymerizable compound U has an amide group, the polymerizable compound U may be, for example, R—C(═O)—NR N - a group represented by *, or *-C(=O)-NR NThe group represented by -R may contain an amide group. R represents a hydrogen atom or a monovalent substituent, preferably a hydrogen atom or a hydrocarbon group, and more preferably a hydrogen atom, an alkyl group, or an aromatic hydrocarbon group. The polymerizable compound U may have two or more structures selected from the group consisting of a hydroxy group, an alkyleneoxy group (however, when a polyalkyleneoxy group is formed, the structure is a polyalkyleneoxy group), an amide group, and a cyano group in the molecule, but an embodiment in which only one structure is present in the molecule is also preferred. The hydroxy group, alkyleneoxy group, amide group, and cyano group may be present at any position in the polymerizable compound U, but from the viewpoint of chemical resistance, it is also preferred that the polymerizable compound U has at least one structure selected from the group consisting of a hydroxy group, an alkyleneoxy group, an amide group, and a cyano group linked to at least one radically polymerizable group contained in the polymerizable compound U via a linking group containing a urea bond or a urethane bond (hereinafter also referred to as "linking group L2-1"). In particular, when the polymerizable compound U contains only one radically polymerizable group, it is preferable that the radically polymerizable group contained in the polymerizable compound U and at least one selected from the group consisting of a hydroxy group, an alkyleneoxy group, an amide group, and a cyano group are linked via a linking group containing a urea bond or a urethane bond (hereinafter also referred to as "linking group L2-2"). When the polymerizable compound U contains an alkyleneoxy group (however, when forming a polyalkyleneoxy group, it is a polyalkyleneoxy group) and has the linking group L2-1 or the linking group L2-2, the structure bonded to the side of the alkyleneoxy group (however, when forming a polyalkyleneoxy group, it is a polyalkyleneoxy group) opposite the linking group L2-1 or the linking group L2-2 is not particularly limited, but is preferably a hydrocarbon group, a radically polymerizable group, or a group represented by a combination thereof. As the hydrocarbon group, a hydrocarbon group having 20 or fewer carbon atoms is preferred, a hydrocarbon group having 18 or fewer carbon atoms is more preferred, and a hydrocarbon group having 16 or fewer carbon atoms is even more preferred. Examples of the hydrocarbon group include a saturated aliphatic hydrocarbon group, an aromatic hydrocarbon group, or a group represented by a bond thereof. Preferred embodiments of the radical polymerizable group are the same as those of the radical polymerizable group in the polymerizable compound U.When the polymerizable compound U contains an amide group and has the linking group L2-1 or L2-2, the structure bonded to the side of the amide group opposite the linking group L2-1 or L2-2 is not particularly limited, but is preferably a hydrocarbon group, a radically polymerizable group, or a group represented by a combination thereof. The hydrocarbon group is preferably a hydrocarbon group having 20 or fewer carbon atoms, more preferably a hydrocarbon group having 18 or fewer carbon atoms, and even more preferably a hydrocarbon group having 16 or fewer carbon atoms. Examples of the hydrocarbon group include saturated aliphatic hydrocarbon groups, aromatic hydrocarbon groups, and groups represented by a bond between these groups. Preferred embodiments of the radically polymerizable group are the same as those of the radically polymerizable group in the polymerizable compound U described above. In the above embodiment, the carbon atom side of the amide group may be bonded to the linking group L2-1 or L2-2, or the nitrogen atom side of the amide group may be bonded to the linking group L2-1 or L2-2. Among these, from the viewpoints of adhesion to the substrate, chemical resistance, and suppression of Cu voids, it is preferable that the polymerizable compound U has a hydroxy group.
[0101] From the viewpoint of compatibility with the specific resin, the polymerizable compound U preferably contains an aromatic group. The aromatic group is preferably directly bonded to a urea bond or a urethane bond contained in the polymerizable compound U. When the polymerizable compound U contains two or more urea bonds or urethane bonds, it is preferable that one of the urea bonds or urethane bonds is directly bonded to the aromatic group. The aromatic group may be an aromatic hydrocarbon group or an aromatic heterocyclic group, or may have a structure in which these form a condensed ring, but is preferably an aromatic hydrocarbon group. The aromatic hydrocarbon group is preferably an aromatic hydrocarbon group having 6 to 30 carbon atoms, more preferably an aromatic hydrocarbon group having 6 to 20 carbon atoms, and even more preferably a group in which two or more hydrogen atoms have been removed from a benzene ring structure. The aromatic heterocyclic group is preferably a 5- or 6-membered aromatic heterocyclic group. Examples of the aromatic heterocyclic ring in such an aromatic heterocyclic group include pyrrole, imidazole, triazole, tetrazole, pyrazole, furan, thiophene, oxazole, isoxazole, thiazole, pyridine, pyrazine, pyrimidine, pyridazine, and triazine. These rings may be condensed with other rings, such as indole and benzimidazole. The heteroatom contained in the aromatic heterocyclic group is preferably a nitrogen atom, an oxygen atom, or a sulfur atom. The aromatic group is preferably contained in a linking group that links two or more radical polymerizable groups and contains a urea bond or a urethane bond, or in a linking group that links at least one selected from the group consisting of the hydroxy group, alkyleneoxy group, amide group, and cyano group to at least one radical polymerizable group contained in the polymerizable compound U.
[0102] The number of atoms (linking chain length) between the urea bond or urethane bond and the radical polymerizable group in the polymerizable compound U is not particularly limited, but is preferably 30 or less, more preferably 2 to 20, and even more preferably 2 to 10. When the polymerizable compound U contains a total of two or more urea bonds or urethane bonds, when it contains two or more radical polymerizable groups, or when it contains two or more urea bonds or urethane bonds and two or more radical polymerizable groups, the minimum number of atoms (linking chain length) between the urea bond or urethane bond and the radical polymerizable group may be within the above range. In this specification, the "number of atoms (linking chain length) between the urea bond or urethane bond and the polymerizable group" refers to the atomic chain on the path connecting the two atoms or atomic groups to be linked that connects these objects via the shortest distance (minimum number of atoms). For example, in the structure represented by the following formula, the number of atoms (linking chain length) between the urea bond and the radical polymerizable group (methacryloyloxy group) is 2.
[0103] [Axis of symmetry] The polymerizable compound U is also preferably a compound having a structure without an axis of symmetry. The polymerizable compound U having no axis of symmetry means that the polymerizable compound U is a bilaterally asymmetric compound having no axis along which the same molecule as the original molecule is generated by rotating the entire compound. Furthermore, when the structural formula of the polymerizable compound U is written on paper, the polymerizable compound U having no axis of symmetry means that the structural formula of the polymerizable compound U cannot be written in a form having an axis of symmetry. It is believed that the absence of an axis of symmetry in the polymerizable compound U suppresses aggregation of the polymerizable compounds U within the composition film.
[0104] [Molecular Weight] The molecular weight of the polymerizable compound U is preferably 100 to 2,000, more preferably 150 to 1,500, and even more preferably 200 to 900.
[0105] The method for producing the polymerizable compound U is not particularly limited, but for example, the polymerizable compound U can be obtained by reacting a radical polymerizable compound and a compound having an isocyanate group with a compound having at least one of a hydroxy group and an amino group.
[0106] Specific examples of the polymerizable compound U are shown below, but the polymerizable compound U is not limited to these.
[0107] From the viewpoints of pattern resolution and film stretchability, the resin composition preferably uses a bifunctional methacrylate or acrylate. Specific compounds include triethylene glycol diacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, tetraethylene glycol diacrylate, PEG (polyethylene glycol) 200 diacrylate, PEG 200 dimethacrylate, PEG 600 diacrylate, PEG 600 dimethacrylate, polytetraethylene glycol diacrylate, polytetraethylene glycol dimethacrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, neopentyl glycol diacrylate, neopentyl glycol dimethacrylate, 3-methyl-1,5-pentanediol diacrylate, 1,6-hexyl ... Examples of usable diacrylates include xanediol diacrylate, 1,6-hexanediol dimethacrylate, dimethylol-tricyclodecane diacrylate, dimethylol-tricyclodecane dimethacrylate, ethylene oxide (EO) adduct diacrylate of bisphenol A, propylene oxide (PO) adduct dimethacrylate of bisphenol A, propylene oxide (PO) adduct dimethacrylate of bisphenol A, 2-hydroxy-3-acryloyloxypropyl methacrylate, EO-modified isocyanuric acid diacrylate, EO-modified isocyanuric acid dimethacrylate, and other bifunctional acrylates and bifunctional methacrylates having urethane bonds. Two or more of these may be mixed and used as needed. For example, PEG200 diacrylate refers to polyethylene glycol diacrylate having a formula weight of approximately 200 for the polyethylene glycol chain. In the resin composition of the present invention, from the viewpoint of suppressing warpage of a pattern (cured product), a polymerizable compound having only one ethylenically unsaturated bond (monofunctional polymerizable compound) can be preferably used as the polymerizable compound having an ethylenically unsaturated bond.Preferred examples of monofunctional polymerizable compounds include (meth)acrylic acid derivatives such as n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, carbitol (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, N-methylol (meth)acrylamide, glycidyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, and polypropylene glycol mono(meth)acrylate; N-vinyl compounds such as N-vinylpyrrolidone and N-vinylcaprolactam; and allyl glycidyl ether. Preferred monofunctional polymerizable compounds include compounds having a boiling point of 100°C or higher under normal pressure in order to suppress volatilization before exposure. Other preferred polymerizable compounds having two or more ethylenically unsaturated bonds include allyl compounds such as diallyl phthalate and triallyl trimellitate.
[0108] The content of the polymerizable compound having an ethylenically unsaturated bond is preferably more than 0% by mass and not more than 60% by mass, more preferably 5% by mass or more, and more preferably 50% by mass or less, and even more preferably 30% by mass or less, based on the total solid content of the resin composition.
[0109] The polymerizable compound having an ethylenically unsaturated bond may be used alone or in combination of two or more. When two or more types are used in combination, the total amount thereof is preferably within the above range.
[0110] [Other Polymerizable Compounds] The resin composition of the present invention preferably further contains another polymerizable compound different from the polymerizable compound having an ethylenically unsaturated bond described above. The other polymerizable compound refers to a polymerizable compound other than the polymerizable compound having an ethylenically unsaturated bond described above. Preferably, the other polymerizable compound has a plurality of groups in the molecule that promote the reaction of forming a covalent bond with other compounds in the composition or their reaction products upon exposure to light by the above-mentioned photoacid generator or photobase generator. Preferably, the other polymerizable compound has a plurality of groups in the molecule that promote the reaction of forming a covalent bond with other compounds in the composition or their reaction products under the action of an acid or base. Examples of other polymerizable compounds include the compounds described in paragraphs 0179 to 0207 of WO 2022 / 145355. The above descriptions are incorporated herein by reference.
[0111] [Polymerization initiator] The resin composition of the present invention preferably contains a polymerization initiator. The polymerization initiator may be a thermal polymerization initiator or a photopolymerization initiator, but it is particularly preferable to contain a photopolymerization initiator. The photopolymerization initiator is preferably a photoradical polymerization initiator. There are no particular restrictions on the photoradical polymerization initiator, and it can be appropriately selected from known photoradical polymerization initiators. For example, a photoradical polymerization initiator that is photosensitive to light in the ultraviolet to visible range is preferred. Alternatively, it may be an activator that reacts with a photoexcited sensitizer to generate active radicals.
[0112] The photoradical polymerization initiator has a capacity of at least about 50 L·mol within a wavelength range of about 240 to 800 nm (preferably 330 to 500 nm). -1 ・cm -1 The molar absorption coefficient of the compound can be measured using a known method. For example, it is preferable to measure the molar absorption coefficient using an ultraviolet-visible spectrophotometer (Varian Cary-5 spectrophotometer) at a concentration of 0.01 g / L using ethyl acetate as a solvent.
[0113] Any known compound can be used as the photoradical polymerization initiator. Examples include halogenated hydrocarbon derivatives (e.g., compounds having a triazine skeleton, compounds having an oxadiazole skeleton, compounds having a trihalomethyl group, etc.), acylphosphine compounds such as acylphosphine oxide, hexaarylbiimidazole, oxime compounds such as oxime derivatives, organic peroxides, thio compounds, ketone compounds, aromatic onium salts, ketoxime ethers, α-aminoketone compounds such as aminoacetophenone, α-hydroxyketone compounds such as hydroxyacetophenone, azo compounds, azide compounds, metallocene compounds, organic boron compounds, and iron arene complexes. For details of these compounds, please refer to paragraphs
[0165] to
[0182] of JP 2016-027357 A and paragraphs
[0138] to
[0151] of WO 2015 / 199219 A, the contents of which are incorporated herein by reference. Further, paragraphs 0065 to 0111 of JP 2014-130173 A, compounds described in Japanese Patent No. 6301489, MATERIAL STAGE 37 to 60p, vol. 19, No. 3,2019 described peroxide-based photopolymerization initiators, photopolymerization initiators described in WO 2018 / 221177, photopolymerization initiators described in WO 2018 / 110179, photopolymerization initiators described in JP 2019-043864 A, photopolymerization initiators described in JP 2019-044030 A, peroxide-based initiators described in JP 2019-167313 A can be mentioned, the contents of which are incorporated herein by reference.
[0114] Examples of ketone compounds include the compounds described in paragraph 0087 of JP 2015-087611 A, the contents of which are incorporated herein by reference. As a commercially available product, Kayacure-DETX-S (manufactured by Nippon Kayaku Co., Ltd.) is also preferably used.
[0115] In one embodiment of the present invention, a hydroxyacetophenone compound, an aminoacetophenone compound, or an acylphosphine compound can be suitably used as the photoradical polymerization initiator. More specifically, for example, an aminoacetophenone-based initiator described in JP-A-10-291969 or an acylphosphine oxide-based initiator described in Japanese Patent No. 4225898 can be used, the contents of which are incorporated herein by reference.
[0116] Examples of α-hydroxyketone initiators that can be used include Omnirad 184, Omnirad 1173, Omnirad 2959, and Omnirad 127 (all manufactured by IGM Resins B.V.), IRGACURE 184 (IRGACURE is a registered trademark), DAROCUR 1173, IRGACURE 500, IRGACURE-2959, and IRGACURE 127 (all manufactured by BASF).
[0117] Examples of α-aminoketone initiators that can be used include Omnirad 907, Omnirad 369, Omnirad 369E, and Omnirad 379EG (all manufactured by IGM Resins B.V.), and IRGACURE 907, IRGACURE 369, and IRGACURE 379 (all manufactured by BASF).
[0118] As the aminoacetophenone initiator, acylphosphine oxide initiator, and metallocene compound, for example, compounds described in paragraphs 0161 to 0163 of WO 2021 / 112189 can also be suitably used. The contents of this specification are incorporated herein by reference.
[0119] As the photoradical polymerization initiator, an oxime compound is more preferably used. By using an oxime compound, it is possible to more effectively improve the exposure latitude. An oxime compound is particularly preferred because it has a wide exposure latitude (exposure margin) and also functions as a photocuring accelerator.
[0120] Specific examples of the oxime compound include compounds described in JP-A-2001-233842, compounds described in JP-A-2000-080068, compounds described in JP-A-2006-342166, compounds described in J. C. S. Perkin II (1979, pp. 1653-1660), compounds described in J. C. S. Perkin II (1979, pp. 156-162), compounds described in Journal of Photopolymer Science and Technology (1995, pp.202-232) described compounds, compounds described in JP-A-2000-066385, compounds described in JP-T-2004-534797, compounds described in JP-A-2017-019766, compounds described in Japanese Patent No. 6065596, compounds described in WO 2015 / 152153, compounds described in WO 2017 / 051680, compounds described in JP-A-2017-198865, compounds described in paragraphs 0025 to 0038 of WO 2017 / 164127, compounds described in WO 2013 / 167515 and the like, the contents of which are incorporated herein.
[0121] Preferred oxime compounds include, for example, compounds having the following structure: 3-(benzoyloxy(imino))butan-2-one, 3-(acetoxy(imino))butan-2-one, 3-(propionyloxy(imino))butan-2-one, 2-(acetoxy(imino))pentan-3-one, 2-(acetoxy(imino))-1-phenylpropan-1-one, 2-(benzoyloxy(imino))-1-phenylpropan-1-one, 3-((4-toluenesulfonyloxy)imino)butan-2-one, and 2-(ethoxycarbonyloxy(imino))-1-phenylpropan-1-one. In the resin composition, it is particularly preferable to use an oxime compound as a photoradical polymerization initiator. The oxime compound as a photoradical polymerization initiator has a linking group of >C=N-O-C(=O)- in the molecule.
[0122]
[0123] Commercially available oxime compounds include IRGACURE OXE 01, IRGACURE OXE 02, IRGACURE OXE 03, and IRGACURE OXE 04 (manufactured by BASF), ADEKA OPTOMER N-1919 (manufactured by ADEKA Corporation, photoradical polymerization initiator 2 described in JP 2012-014052 A), TR-PBG-304, TR-PBG-305 (manufactured by Changzhou Strong Electronic New Materials Co., Ltd.), ADEKA ARCLES NCI-730, NCI-831, and ADEKA ARCLES NCI-930 (manufactured by ADEKA Corporation), DFI-091 (manufactured by Daito ChemiX Co., Ltd.), and SpeedCure PDO (SARTOMER Also, an oxime compound having the following structure can be used.
[0124] Examples of photoradical polymerization initiators include oxime compounds having a fluorene ring, oxime compounds having a skeleton in which at least one benzene ring of a carbazole ring is replaced with a naphthalene ring, and oxime compounds having a fluorine atom, as described in paragraphs 0169 to 0171 of WO 2021 / 112189. Also usable are oxime compounds having a nitro group, oxime compounds having a benzofuran skeleton, and oxime compounds in which a substituent having a hydroxy group is bonded to a carbazole skeleton, as described in paragraphs 0208 to 0210 of WO 2021 / 020359. The contents of these compounds are incorporated herein by reference.
[0125] As the photopolymerization initiator, an aromatic ring group Ar in which an electron-withdrawing group is introduced into the aromatic ring can be used. OX1 It is also possible to use an oxime compound having the aromatic ring group Ar OX1Examples of the electron-withdrawing group include an acyl group, a nitro group, a trifluoromethyl group, an alkylsulfinyl group, an arylsulfinyl group, an alkylsulfonyl group, an arylsulfonyl group, and a cyano group. Acyl and nitro groups are preferred, and an acyl group is more preferred because it is easier to form a film with excellent light resistance, and a benzoyl group is even more preferred. The benzoyl group may have a substituent. The substituent is preferably a halogen atom, a cyano group, a nitro group, a hydroxy group, an alkyl group, an alkoxy group, an aryl group, an aryloxy group, a heterocyclic group, a heterocyclic oxy group, an alkenyl group, an alkylsulfanyl group, an arylsulfanyl group, an acyl group, or an amino group. An alkyl group, an alkoxy group, an aryl group, an aryloxy group, a heterocyclic oxy group, an alkylsulfanyl group, an arylsulfanyl group, or an amino group is more preferred, and an alkoxy group, an alkylsulfanyl group, or an amino group is even more preferred.
[0126] The oxime compound OX is preferably at least one selected from the compounds represented by formula (OX1) and the compounds represented by formula (OX2), and more preferably the compound represented by formula (OX2). In the formula, R X1 represents an alkyl group, an alkenyl group, an alkoxy group, an aryl group, an aryloxy group, a heterocyclic group, a heterocyclic oxy group, an alkylsulfanyl group, an arylsulfanyl group, an alkylsulfinyl group, an arylsulfinyl group, an alkylsulfonyl group, an arylsulfonyl group, an acyl group, an acyloxy group, an amino group, a phosphinoyl group, a carbamoyl group or a sulfamoyl group; R X2 represents an alkyl group, an alkenyl group, an alkoxy group, an aryl group, an aryloxy group, a heterocyclic group, a heterocyclic oxy group, an alkylsulfanyl group, an arylsulfanyl group, an alkylsulfinyl group, an arylsulfinyl group, an alkylsulfonyl group, an arylsulfonyl group, an acyloxy group, or an amino group; R X3 ~R X14 each independently represents a hydrogen atom or a substituent. X10 ~R X14At least one of the groups is an electron-withdrawing group.
[0127] In the above formula, R X12 is an electron-withdrawing group, and R X10 , R X11 , R X13 , R X14 is preferably a hydrogen atom.
[0128] Specific examples of the oxime compound OX include the compounds described in paragraphs 0083 to 0105 of Japanese Patent No. 4600600, the contents of which are incorporated herein by reference.
[0129] Particularly preferred oxime compounds include oxime compounds having specific substituents as disclosed in JP-A-2007-269779 and oxime compounds having a thioaryl group as disclosed in JP-A-2009-191061, the contents of which are incorporated herein by reference.
[0130] From the viewpoint of exposure sensitivity, the photoradical polymerization initiator is preferably a compound selected from the group consisting of trihalomethyltriazine compounds, benzyl dimethyl ketal compounds, α-hydroxyketone compounds, α-aminoketone compounds, acylphosphine compounds, phosphine oxide compounds, metallocene compounds, oxime compounds, triarylimidazole dimers, onium salt compounds, benzothiazole compounds, benzophenone compounds, acetophenone compounds and derivatives thereof, cyclopentadiene-benzene-iron complexes and salts thereof, halomethyloxadiazole compounds, and 3-aryl-substituted coumarin compounds.
[0131] The photoradical polymerization initiator is a trihalomethyltriazine compound, an α-aminoketone compound, an acylphosphine compound, a phosphine oxide compound, a metallocene compound, an oxime compound, a triarylimidazole dimer, an onium salt compound, a benzophenone compound, or an acetophenone compound, more preferably at least one compound selected from the group consisting of a trihalomethyltriazine compound, an α-aminoketone compound, a metallocene compound, an oxime compound, a triarylimidazole dimer, or a benzophenone compound, and even more preferably a metallocene compound or an oxime compound.
[0132] As the photoradical polymerization initiator, the compounds described in paragraphs 0175 to 0179 of WO 2021 / 020359 and the compounds described in paragraphs 0048 to 0055 of WO 2015 / 125469 can also be used, the contents of which are incorporated herein by reference.
[0133] As the photoradical polymerization initiator, a bifunctional or trifunctional or higher functional photoradical polymerization initiator may be used. By using such a photoradical polymerization initiator, two or more radicals are generated from one molecule of the photoradical polymerization initiator, thereby obtaining good sensitivity. Furthermore, when a compound with an asymmetric structure is used, crystallinity is reduced and solubility in solvents is improved, making it less likely to precipitate over time, and improving the stability of the resin composition over time. Specific examples of the bifunctional or trifunctional or higher functional photoradical polymerization initiator include dimers of oxime compounds described in JP-T-2010-527339, JP-T-2011-524436, WO 2015 / 004565, WO 2016-532675, paragraphs 0407 to 0412, and WO 2017 / 033680, paragraphs 0039 to 0055; compounds (E) and (G) described in JP-T-2013-522445; oxime ester photoinitiators described in paragraph 0007 of JP-T-2017-523465, photoinitiators described in paragraphs 0020 to 0033 of JP-A-2017-167399, photopolymerization initiator (A) described in paragraphs 0017 to 0026 of JP-A-2017-151342, and oxime ester photoinitiators described in Japanese Patent No. 6469669, the contents of which are incorporated herein by reference.
[0134] When the resin composition contains a photopolymerization initiator, the content thereof is preferably 0.1 to 30% by mass, more preferably 0.1 to 20% by mass, even more preferably 0.5 to 15% by mass, and even more preferably 1.0 to 10% by mass, based on the total solid content of the resin composition. Only one type of photopolymerization initiator may be contained, or two or more types may be contained. When two or more types of photopolymerization initiators are contained, the total amount is preferably within the above range. Note that the photopolymerization initiator may also function as a thermal polymerization initiator, and therefore crosslinking by the photopolymerization initiator may be further promoted by heating in an oven, hot plate, or the like.
[0135] [Sensitizer] The resin composition may contain a sensitizer. The sensitizer absorbs specific actinic radiation and becomes electronically excited. The electronically excited sensitizer comes into contact with a thermal radical polymerization initiator, a photoradical polymerization initiator, or the like, and undergoes electron transfer, energy transfer, heat generation, and other actions. This causes the thermal radical polymerization initiator or the photoradical polymerization initiator to undergo a chemical change and decompose, generating a radical, acid, or base. Usable sensitizers include benzophenone-based, Michler's ketone-based, coumarin-based, pyrazole azo-based, anilino azo-based, triphenylmethane-based, anthraquinone-based, anthracene-based, anthrapyridone-based, benzylidene-based, oxonol-based, pyrazolotriazole azo-based, pyridone azo-based, cyanine-based, phenothiazine-based, pyrrolopyrazole azomethine-based, xanthene-based, phthalocyanine-based, benzopyran-based, and indigo-based compounds.Examples of the sensitizer include Michler's ketone, 4,4'-bis(diethylamino)benzophenone, 2,5-bis(4'-diethylaminobenzal)cyclopentane, 2,6-bis(4'-diethylaminobenzal)cyclohexanone, 2,6-bis(4'-diethylaminobenzal)-4-methylcyclohexanone, 4,4'-bis(dimethylamino)chalcone, 4,4'-bis(diethylamino)chalcone, p-dimethylaminocinnamylideneindanone, p-dimethylaminobenzylideneindanone, and Non, 2-(p-dimethylaminophenylbiphenylene)benzothiazole, 2-(p-dimethylaminophenylvinylene)benzothiazole, 2-(p-dimethylaminophenylvinylene)isonaphthothiazole, 1,3-bis(4'-dimethylaminobenzal)acetone, 1,3-bis(4'-diethylaminobenzal)acetone, 3,3'-carbonyl-bis(7-diethylaminocoumarin), 3-acetyl-7-dimethylaminocoumarin, 3-ethoxycarbonyl-7-dimethylaminocoumarin Phosphorus, 3-benzyloxycarbonyl-7-dimethylaminocoumarin, 3-methoxycarbonyl-7-diethylaminocoumarin, 3-ethoxycarbonyl-7-diethylaminocoumarin (ethyl 7-(diethylamino)coumarin-3-carboxylate), N-phenyl-N'-ethylethanolamine, N-phenyldiethanolamine, N-p-tolyldiethanolamine, N-phenylethanolamine, 4-morpholinobenzophenone, isoamyl dimethylaminobenzoate, isoamyl diethylaminobenzoate Examples of sensitizing dyes include soamyl, 2-mercaptobenzimidazole, 1-phenyl-5-mercaptotetrazole, 2-mercaptobenzothiazole, 2-(p-dimethylaminostyryl)benzoxazole, 2-(p-dimethylaminostyryl)benzothiazole, 2-(p-dimethylaminostyryl)naphtho(1,2-d)thiazole, 2-(p-dimethylaminobenzoyl)styrene, diphenylacetamide, benzanilide, N-methylacetanilide, and 3',4'-dimethylacetanilide. Other sensitizing dyes may also be used. For details of sensitizing dyes, please refer to the descriptions in paragraphs 0161 to 0163 of JP-A-2016-027357, the contents of which are incorporated herein by reference.
[0136] When the resin composition contains a sensitizer, the content of the sensitizer is preferably 0.01 to 20 mass %, more preferably 0.1 to 15 mass %, and still more preferably 0.5 to 10 mass %, based on the total solid content of the resin composition. The sensitizer may be used alone or in combination of two or more types.
[0137] [Chain Transfer Agent] The resin composition of the present invention may contain a chain transfer agent. Chain transfer agents are defined, for example, in the Third Edition of the Polymer Dictionary (edited by the Society of Polymer Science, 2005), pages 683-684. Examples of chain transfer agents include those having -S-S-, -SO 2 Examples of compounds that can be used include compounds having -S-, -N-O-, SH, PH, SiH, and GeH, and dithiobenzoates, trithiocarbonates, dithiocarbamates, and xanthate compounds having a thiocarbonylthio group used in RAFT (Reversible Addition Fragmentation Chain Transfer) polymerization. These compounds can donate hydrogen to low-activity radicals to generate radicals, or can be oxidized and then deprotonated to generate radicals. Thiol compounds are particularly preferred.
[0138] In addition, the chain transfer agent may be a compound described in paragraphs 0152 to 0153 of WO 2015 / 199219, the contents of which are incorporated herein by reference.
[0139] When the resin composition contains a chain transfer agent, the content of the chain transfer agent is preferably 0.01 to 20 parts by mass, more preferably 0.1 to 10 parts by mass, and even more preferably 0.5 to 5 parts by mass, relative to 100 parts by mass of the total solid content of the resin composition. Only one type of chain transfer agent may be used, or two or more types may be used. When two or more types of chain transfer agents are used, the total content thereof is preferably within the above range.
[0140] A photoacid generator may also be used as the photopolymerization initiator. The photoacid generator is preferably a photoacid generator that generates radicals. Specifically, it is preferably a compound that absorbs light, decomposes to generate radicals, and abstracts hydrogen from a solvent, the acid generator itself, or the like to generate an acid.
[0141] Examples of the photoacid generator include quinone diazide compounds, oxime sulfonate compounds, organic halide compounds, organic borate compounds, disulfone compounds, and onium salts, and onium salts are preferred. Examples of the onium salts include diazonium salts, phosphonium salts, sulfonium salts, and iodonium salts.
[0142] Furthermore, the onium salt is a salt of a cation and an anion having an onium structure, and the cation and the anion may or may not be bonded via a covalent bond. That is, the onium salt may be an intramolecular salt having a cation moiety and an anion moiety in the same molecular structure, or an intermolecular salt in which a cation molecule and an anion molecule, which are separate molecules, are ionically bonded, but an intermolecular salt is preferred. Furthermore, in the composition of the present invention, the cation moiety or the cation molecule and the anion moiety or the anion molecule may be bonded via an ionic bond or may be dissociated.
[0143] [Sulfonium Salt] In the present invention, the sulfonium salt means a salt of a sulfonium cation and an anion.
[0144] -Sulfonium Cation- As the sulfonium cation, a tertiary sulfonium cation is preferable, and a triaryl sulfonium cation is more preferable. Furthermore, as the sulfonium cation, a cation represented by the following formula (103) is preferable.
[0145] In formula (103), R 8 ~R 10 R each independently represents a hydrocarbon group. 8 ~R 10 are each independently preferably an alkyl group or an aryl group, more preferably an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 12 carbon atoms, even more preferably an aryl group having 6 to 12 carbon atoms, and even more preferably a phenyl group. 8 ~R 10may have a substituent, and examples of the substituent include a hydroxy group, an aryl group, an alkoxy group, an aryloxy group, an arylcarbonyl group, an alkylcarbonyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, and an acyloxy group. Among these, it is preferable that the substituent is an alkyl group or an alkoxy group, more preferably a branched alkyl group or an alkoxy group, and even more preferably a branched alkyl group having 3 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms. R 8 ~R 10 may be the same group or different groups, but from the viewpoint of synthetic suitability, they are preferably the same group.
[0146] -Anion- The anion is not particularly limited and may be selected in consideration of the acid to be generated. 6 F 5 ) 4 - , B.F. 4 - Boron-based anions such as (Rf) n PF 6-n - 、 PF 3 (C 2 F 5 ) 3- , P.F. 6 - phosphorus-based anions such as SbF 6 - and other anions such as carboxylate anions and sulfonate anions.
[0147] [Iodonium Salt] In the present invention, the iodonium salt refers to a salt of an iodonium cation and an anion. Examples of the anion include the same anions as those in the sulfonium salt described above, and preferred embodiments are also the same.
[0148] -Iodonium Cation- As the iodonium cation, a diaryliodonium cation is preferred. Furthermore, as the iodonium cation, a cation represented by the following formula (104) is preferred.
[0149] In formula (104), R 11 and R 12 R each independently represents a hydrocarbon group. 11 and R 12 are each independently preferably an alkyl group or an aryl group, more preferably an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 12 carbon atoms, even more preferably an aryl group having 6 to 12 carbon atoms, and even more preferably a phenyl group. 11 and R 12 may have a substituent, and examples of the substituent include a hydroxy group, an aryl group, an alkoxy group, an aryloxy group, an arylcarbonyl group, an alkylcarbonyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, and an acyloxy group. Among these, it is preferable that the substituent is an alkyl group or an alkoxy group, more preferably a branched alkyl group or an alkoxy group, and even more preferably a branched alkyl group having 3 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms. R 11 and R 12 may be the same group or different groups, but from the viewpoint of synthetic suitability, they are preferably the same group.
[0150] [Phosphonium Salt] In the present invention, the phosphonium salt refers to a salt of a phosphonium cation and an anion. Examples of the anion include the same anions as those in the sulfonium salt described above, and preferred embodiments are also the same.
[0151] -Phosphonium Cation- The phosphonium cation is preferably a quaternary phosphonium cation, such as a tetraalkylphosphonium cation, a triarylmonoalkylphosphonium cation, etc. Furthermore, the phosphonium cation is preferably a cation represented by the following formula (105):
[0152] In formula (105), R 13 ~R 16 R each independently represents a hydrogen atom or a hydrocarbon group. 13 ~R 16are each independently preferably an alkyl group or an aryl group, more preferably an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 12 carbon atoms, even more preferably an aryl group having 6 to 12 carbon atoms, and even more preferably a phenyl group. 13 ~R 16 may have a substituent, and examples of the substituent include a hydroxy group, an aryl group, an alkoxy group, an aryloxy group, an arylcarbonyl group, an alkylcarbonyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, and an acyloxy group. Among these, it is preferable that the substituent is an alkyl group or an alkoxy group, more preferably a branched alkyl group or an alkoxy group, and even more preferably a branched alkyl group having 3 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms. R 13 ~R 16 may be the same group or different groups, but from the viewpoint of synthetic suitability, they are preferably the same group.
[0153] The content of the photoacid generator is preferably 0.1 to 20% by mass, more preferably 0.5 to 18% by mass, even more preferably 0.5 to 10% by mass, even more preferably 0.5 to 3% by mass, and even more preferably 0.5 to 1.2% by mass, based on the total solid content of the resin composition. The photoacid generator may be used alone or in combination with multiple types. In the case of a combination of multiple types, it is preferable that the total amount thereof is within the above range. It is also preferable to use it in combination with a sensitizer to impart photosensitivity to a desired light source.
[0154] In another preferred embodiment of the present invention, the resin composition of the present invention contains two or more polymerization initiators. Specifically, the resin composition of the present invention preferably contains a photopolymerization initiator and a thermal polymerization initiator described below, or the above-mentioned photoradical polymerization initiator and the above-mentioned photoacid generator.
[0155] By including a photopolymerization initiator and a thermal polymerization initiator described below, pattern formation by exposure becomes possible, and radical polymerization also proceeds more easily during curing by a heating step described below, which may improve performance such as chemical resistance. When a photopolymerization initiator and a thermal polymerization initiator described below are included, the content of the thermal polymerization initiator is preferably 20 to 70% by mass, and more preferably 30 to 60% by mass, relative to the total content of the photopolymerization initiator and the thermal polymerization initiator.
[0156] Inclusion of a photoradical polymerization initiator and a photoacid generator may improve performance such as resolution. When a photopolymerization initiator and a photoacid generator are included, the content ratio of the photoacid generator relative to the total content of the photopolymerization initiator and the photoacid generator is preferably 20 to 70 mass %, more preferably 30 to 60 mass %.
[0157] [Thermal Polymerization Initiator] Examples of the thermal polymerization initiator include a thermal radical polymerization initiator. A thermal radical polymerization initiator is a compound that generates radicals by thermal energy and initiates or promotes the polymerization reaction of a polymerizable compound. Addition of a thermal radical polymerization initiator can also promote the polymerization reaction of the resin and the polymerizable compound, thereby further improving solvent resistance.
[0158] Specific examples of the thermal radical polymerization initiator include compounds described in paragraphs 0074 to 0118 of JP-A-2008-063554, the contents of which are incorporated herein by reference.
[0159] When a thermal polymerization initiator is contained, the content thereof is preferably 0.1 to 30 mass% relative to the total solid content of the resin composition, more preferably 0.1 to 20 mass%, and even more preferably 0.5 to 15 mass%. The resin composition may contain only one type of thermal polymerization initiator, or may contain two or more types. When two or more types of thermal polymerization initiators are contained, the total amount is preferably in the above range.
[0160] <Base Generator> The resin composition of the present invention may contain a base generator. Here, the base generator is a compound capable of generating a base by physical or chemical action. Preferred base generators include thermal base generators and photobase generators. In particular, when the resin composition contains a precursor of a cyclized resin, the resin composition preferably contains a base generator. By containing a thermal base generator in the resin composition, the cyclization reaction of the precursor can be promoted, for example, by heating, and the mechanical properties and chemical resistance of the cured product can be improved, resulting in excellent performance as an interlayer insulating film for a rewiring layer included in a semiconductor package. The base generator may be an ionic base generator or a nonionic base generator. Examples of the base generated from the base generator include secondary amines and tertiary amines. The base generator is not particularly limited, and known base generators can be used. Examples of known base generators include carbamoyl oxime compounds, carbamoyl hydroxylamine compounds, carbamic acid compounds, formamide compounds, acetamide compounds, carbamate compounds, benzyl carbamate compounds, nitrobenzyl carbamate compounds, sulfonamide compounds, imidazole derivative compounds, amine imide compounds, pyridine derivative compounds, α-aminoacetophenone derivative compounds, quaternary ammonium salt derivative compounds, iminium salts, pyridinium salts, α-lactone ring derivative compounds, amine imide compounds, phthalimide derivative compounds, and acyloxyimino compounds. Specific examples of non-ionic base generators include the compounds described in paragraphs 0249 to 0275 of WO 2022 / 145355. The above descriptions are incorporated herein by reference.
[0161] Examples of the base generator include, but are not limited to, the following compounds:
[0162]
[0163] The molecular weight of the nonionic base generator is preferably 800 or less, more preferably 600 or less, and even more preferably 500 or less. The lower limit is preferably 100 or more, more preferably 200 or more, and even more preferably 300 or more.
[0164] Specific preferred compounds for the ionic base generator include, for example, the compounds described in paragraphs 0148 to 0163 of WO 2018 / 038002.
[0165] Specific examples of ammonium salts include, but are not limited to, the following compounds:
[0166] Specific examples of iminium salts include, but are not limited to, the following compounds:
[0167] The base generator is preferably an amine in which the amino group is protected with a t-butoxycarbonyl group, from the viewpoints of storage stability and generating a base by deprotection during curing.
[0168] Examples of amine compounds protected by a t-butoxycarbonyl group include ethanolamine, 3-amino-1-propanol, 1-amino-2-propanol, 2-amino-1-propanol, 4-amino-1-butanol, 2-amino-1-butanol, 1-amino-2-butanol, 3-amino-2,2-dimethyl-1-propanol, 4-amino-2-methyl-1-butanol, valinol, 3-amino-1,2-propanediol, and 2-amino-1,3-propanediol. alcohol, tyramine, norephedrine, 2-amino-1-phenyl-1,3-propanediol, 2-aminocyclohexanol, 4-aminocyclohexanol, 4-aminocyclohexaneethanol, 4-(2-aminoethyl)cyclohexanol, N-methylethanolamine, 3-(methylamino)-1-propanol, 3-(isopropylamino)propanol, N-cyclohexylethanolamine, α-[2-(methylamino)ethyl]benzyl alcohol, diethanolamine diamine, diisopropanolamine, 3-pyrrolidinol, 2-pyrrolidinemethanol, 4-hydroxypiperidine, 3-hydroxypiperidine, 4-hydroxy-4-phenylpiperidine, 4-(3-hydroxyphenyl)piperidine, 4-piperidinemethanol, 3-piperidinemethanol, 2-piperidinemethanol, 4-piperidineethanol, 2-piperidineethanol, 2-(4-piperidyl)-2-propanol, 1,4-butanolbis(3-aminopropyl)ethanol ter, 1,2-bis(2-aminoethoxy)ethane, 2,2'-oxybis(ethylamine), 1,14-diamino-3,6,9,12-tetraoxatetradecane, 1-aza-15-crown-5-ether, diethylene glycol bis(3-aminopropyl)ether, 1,11-diamino-3,6,9-trioxaundecane, or compounds in which the amino group of an amino acid or a derivative thereof is protected with a t-butoxycarbonyl group, but are not limited to these.
[0169] When the resin composition contains a base generator, the content of the base generator is preferably 0.1 to 50 parts by mass per 100 parts by mass of the resin in the resin composition. The lower limit is more preferably 0.3 parts by mass or more, and even more preferably 0.5 parts by mass or more. The upper limit is more preferably 30 parts by mass or less, even more preferably 20 parts by mass or less, even more preferably 10 parts by mass or less, even more preferably 5 parts by mass or less, and particularly preferably 4 parts by mass or less. One or more types of base generators can be used. When two or more types are used, the total amount is preferably within the above range.
[0170] <Solvent> The resin composition of the present invention preferably contains a solvent. Any known solvent can be used as the solvent. The solvent is preferably an organic solvent. Examples of the organic solvent include compounds such as esters, ethers, ketones, cyclic hydrocarbons, sulfoxides, amides, ureas, and alcohols.
[0171] Examples of esters include ethyl acetate, n-butyl acetate, isobutyl acetate, hexyl acetate, amyl formate, isoamyl acetate, butyl propionate, isopropyl butyrate, ethyl butyrate, butyl butyrate, methyl lactate, ethyl lactate, γ-butyrolactone, ε-caprolactone, δ-valerolactone, γ-valerolactone, alkyl alkyloxyacetates (for example, methyl alkyloxyacetate, ethyl alkyloxyacetate, butyl alkyloxyacetate (for example, methyl methoxyacetate, ethyl methoxyacetate, butyl methoxyacetate, methyl ethoxyacetate, ethyl ethoxyacetate, etc.)), 3-alkyloxypropionic acid alkyl esters (for example, methyl 3-alkyloxypropionate, ethyl 3-alkyloxypropionate (for example, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, etc.)), 2-alkyloxypropionic acid alkyl esters ...alkyloxypropionate, ethyl 3-alkyloxypropionate, 2-alkyloxypropionic acid alkyl esters (for example, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, etc.)), 2-alkyloxypropionic acid alkyl esters (for example, methyl 3-alkyloxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, etc.)), 2-alkyloxypropionic acid alkyl esters (for example, methyl 3- Preferred examples thereof include alkyl esters of alkyloxypropionates (e.g., methyl 2-alkyloxypropionate, ethyl 2-alkyloxypropionate, propyl 2-alkyloxypropionate (e.g., methyl 2-methoxypropionate, ethyl 2-methoxypropionate, propyl 2-methoxypropionate, methyl 2-ethoxypropionate, ethyl 2-ethoxypropionate)), methyl 2-alkyloxy-2-methylpropionate and ethyl 2-alkyloxy-2-methylpropionate (e.g., methyl 2-methoxy-2-methylpropionate, ethyl 2-ethoxy-2-methylpropionate), methyl pyruvate, ethyl pyruvate, propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, methyl 2-oxobutanoate, ethyl 2-oxobutanoate, ethyl hexanoate, ethyl heptanoate, dimethyl malonate, and diethyl malonate.
[0172] Suitable examples of ethers include ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol ethyl methyl ether, diethylene glycol butyl methyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, tetrahydrofuran, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol dimethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether, ethylene glycol monobutyl ether acetate, diethylene glycol ethyl methyl ether, propylene glycol monopropyl ether acetate, and dipropylene glycol dimethyl ether.
[0173] Suitable examples of ketones include methyl ethyl ketone, cyclohexanone, cyclopentanone, 2-heptanone, 3-heptanone, 3-methylcyclohexanone, levoglucosenone, and dihydrolevoglucosenone.
[0174] Suitable examples of cyclic hydrocarbons include aromatic hydrocarbons such as toluene, xylene, and anisole, and cyclic terpenes such as limonene.
[0175] A preferred example of the sulfoxides is dimethyl sulfoxide.
[0176] Preferred examples of the amides include N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N-cyclohexyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, N,N-dimethylisobutyramide, 3-methoxy-N,N-dimethylpropionamide, 3-butoxy-N,N-dimethylpropionamide, N-formylmorpholine, and N-acetylmorpholine.
[0177] Preferred examples of ureas include N,N,N',N'-tetramethylurea and 1,3-dimethyl-2-imidazolidinone.
[0178] Examples of alcohols include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 1-pentanol, 1-hexanol, benzyl alcohol, ethylene glycol monomethyl ether, 1-methoxy-2-propanol, 2-ethoxyethanol, diethylene glycol monoethyl ether, diethylene glycol monohexyl ether, triethylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether, polyethylene glycol monomethyl ether, polypropylene glycol, tetraethylene glycol, ethylene glycol monobutyl ether, ethylene glycol monobenzyl ether, ethylene glycol monophenyl ether, methylphenyl carbinol, n-amyl alcohol, methyl amyl alcohol, and diacetone alcohol.
[0179] From the viewpoint of improving the properties of the coated surface, it is also preferable to mix two or more kinds of solvents.
[0180] In the present invention, one solvent selected from methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, ethyl cellosolve acetate, ethyl lactate, diethylene glycol dimethyl ether, butyl acetate, methyl 3-methoxypropionate, 2-heptanone, cyclohexanone, cyclopentanone, γ-butyrolactone, γ-valerolactone, 3-methoxy-N,N-dimethylpropionamide, toluene, dimethyl sulfoxide, ethyl carbitol acetate, butyl carbitol acetate, N-methyl-2-pyrrolidone, propylene glycol methyl ether, propylene glycol methyl ether acetate, levoglucosenone, and dihydrolevoglucosenone, or a mixed solvent composed of two or more solvents, is preferred. Particularly preferred are a combination of dimethyl sulfoxide and γ-butyrolactone, a combination of dimethyl sulfoxide and γ-valerolactone, a combination of 3-methoxy-N,N-dimethylpropionamide and γ-butyrolactone, a combination of 3-methoxy-N,N-dimethylpropionamide, γ-butyrolactone and dimethyl sulfoxide, or a combination of N-methyl-2-pyrrolidone and ethyl lactate. An embodiment in which toluene is further added to these combined solvents in an amount of approximately 1 to 10% by mass, based on the total mass of the solvent, is also a preferred embodiment of the present invention. In particular, from the viewpoint of the storage stability of the resin composition, an embodiment in which γ-valerolactone is included as a solvent is also a preferred embodiment of the present invention. In such an embodiment, the content of γ-valerolactone relative to the total mass of the solvent is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more. The upper limit of the above content is not particularly limited and may be 100% by mass. The above content may be determined taking into consideration the solubility of components such as the specific resin contained in the resin composition, etc. Furthermore, when dimethyl sulfoxide and γ-valerolactone are used in combination, the solvent preferably contains 60 to 90 mass% of γ-valerolactone and 10 to 40 mass% of dimethyl sulfoxide, more preferably 70 to 90 mass% of γ-valerolactone and 10 to 30 mass% of dimethyl sulfoxide, and even more preferably 75 to 85 mass% of γ-valerolactone and 15 to 25 mass% of dimethyl sulfoxide, relative to the total mass of the solvent.
[0181] From the viewpoint of coatability, the content of the solvent is preferably an amount such that the total solids concentration of the resin composition of the present invention is 5 to 80 mass%, more preferably an amount such that the total solids concentration is 5 to 75 mass%, even more preferably an amount such that the total solids concentration is 10 to 70 mass%, and even more preferably an amount such that the total solids concentration is 20 to 70 mass%. The solvent content may be adjusted depending on the desired thickness of the coating film and the coating method. When two or more solvents are contained, the total amount of the solvents is preferably within the above range.
[0182] <Metal Adhesion Improver> The resin composition of the present invention preferably contains a metal adhesion improver from the viewpoint of improving adhesion to metal materials used in electrodes, wiring, etc. Examples of the metal adhesion improver include a silane coupling agent having an alkoxysilyl group, an aluminum-based adhesion aid, a titanium-based adhesion aid, a compound having a sulfonamide structure, a compound having a thiourea structure, a phosphoric acid derivative compound, a β-ketoester compound, and an amino compound.
[0183] [Silane Coupling Agent] Examples of silane coupling agents include the compounds described in paragraph 0316 of WO 2021 / 112189 and the compounds described in paragraphs 0067 to 0078 of JP 2018-173573 A, the contents of which are incorporated herein by reference. It is also preferable to use two or more different silane coupling agents, as described in paragraphs 0050 to 0058 of JP 2011-128358 A. It is also preferable to use the following compounds as the silane coupling agent. In the formula below, Me represents a methyl group, and Et represents an ethyl group. Furthermore, the following R represents a structure derived from a blocking agent in a blocked isocyanate group. The blocking agent may be selected depending on the desorption temperature, and examples include alcohol compounds, phenol compounds, pyrazole compounds, triazole compounds, lactam compounds, and active methylene compounds. For example, caprolactam is preferred from the viewpoint of achieving a desorption temperature of 160 to 180°C. Commercially available products of such compounds include X-12-1293 (manufactured by Shin-Etsu Chemical Co., Ltd.).
[0184]
[0185] Other silane coupling agents include, for example, vinyltrimethoxysilane, vinyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, N-2- Examples of suitable silane coupling agents include (aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, tris-(trimethoxysilylpropyl)isocyanurate, 3-ureidopropyltrialkoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, and 3-trimethoxysilylpropylsuccinic anhydride. These may be used alone or in combination of two or more. Furthermore, oligomeric compounds having multiple alkoxysilyl groups may also be used as silane coupling agents. Examples of such oligomeric compounds include compounds containing a repeating unit represented by the following formula (S-1): In formula (S-1), R S1 represents a monovalent organic group, R S2 represents a hydrogen atom, a hydroxy group or an alkoxy group, and n represents an integer of 0 to 2. S1is preferably a structure containing a polymerizable group. Examples of the polymerizable group include a group having an ethylenically unsaturated bond, an epoxy group, an oxetanyl group, a benzoxazolyl group, a blocked isocyanate group, and an amino group. Examples of the group having an ethylenically unsaturated bond include a vinyl group, an allyl group, an isoallyl group, a 2-methylallyl group, a group having an aromatic ring directly bonded to a vinyl group (for example, a vinylphenyl group), a (meth)acrylamide group, and a (meth)acryloyloxy group. A vinylphenyl group, a (meth)acrylamide group, or a (meth)acryloyloxy group is preferred, a vinylphenyl group or a (meth)acryloyloxy group is more preferred, and a (meth)acryloyloxy group is even more preferred. R S2 is preferably an alkoxy group, more preferably a methoxy group or an ethoxy group. n represents an integer of 0 to 2, preferably 1. Here, the structures of the multiple repeating units represented by formula (S-1) contained in the oligomer-type compound may be the same. Here, of the multiple repeating units represented by formula (S-1) contained in the oligomer-type compound, it is preferable that n is 1 or 2 in at least one, more preferably that n is 1 or 2 in at least two, and even more preferably that n is 1 in at least two. Such oligomer-type compounds can be commercially available products, and an example of a commercially available product is KR-513 (manufactured by Shin-Etsu Chemical Co., Ltd.).
[0186] [Aluminum-Based Adhesion Aid] Examples of aluminum-based adhesion aids include aluminum tris(ethylacetoacetate), aluminum tris(acetylacetonate), and ethylacetoacetate aluminum diisopropylate.
[0187] Other metal adhesion improvers that can be used include the compounds described in paragraphs 0046 to 0049 of JP-A-2014-186186 and the sulfide-based compounds described in paragraphs 0032 to 0043 of JP-A-2013-072935, the contents of which are incorporated herein by reference.
[0188] The content of the metal adhesion improver is preferably 0.01 to 30 parts by mass, more preferably 0.1 to 10 parts by mass, and even more preferably 0.5 to 5 parts by mass, relative to 100 parts by mass of the specific resin. By ensuring that the content is equal to or greater than the above lower limit, the adhesion between the pattern and the metal layer is improved, and by ensuring that the content is equal to or less than the above upper limit, the heat resistance and mechanical properties of the pattern are improved. Only one type of metal adhesion improver may be used, or two or more types may be used. When two or more types are used, it is preferable that the total amount is within the above range.
[0189] <Migration Inhibitor> The resin composition of the present invention preferably further contains a migration inhibitor. By including a migration inhibitor, for example, when the resin composition is applied to a metal layer (or metal wiring) to form a film, migration of metal ions derived from the metal layer (or metal wiring) into the film can be effectively inhibited.
[0190] The migration inhibitor is not particularly limited, but examples thereof include compounds having a heterocycle (pyrrole ring, furan ring, thiophene ring, imidazole ring, oxazole ring, thiazole ring, pyrazole ring, isoxazole ring, isothiazole ring, tetrazole ring, pyridine ring, pyridazine ring, pyrimidine ring, pyrazine ring, piperidine ring, piperazine ring, morpholine ring, 2H-pyran ring, 6H-pyran ring, triazine ring), thioureas and compounds having a sulfanyl group, hindered phenol compounds, salicylic acid derivative compounds, and hydrazide derivative compounds. In particular, triazole compounds such as 1,2,4-triazole, benzotriazole, 3-amino-1,2,4-triazole, and 3,5-diamino-1,2,4-triazole, and tetrazole compounds such as 1H-tetrazole, 5-phenyltetrazole, and 5-amino-1H-tetrazole are preferably used.
[0191] Among these, the resin composition of the present invention preferably contains an azole compound. The azole compound is a compound containing an azole structure, and the azole structure refers to a five-membered ring structure containing a nitrogen atom as a ring member, and preferably a five-membered ring structure containing two or more nitrogen atoms as ring members. Specific examples of the azole structure include an imidazole structure, a triazole structure, and a tetrazole structure. These structures may form a polycycle by condensation with another ring structure, such as benzimidazole or benzotriazole. Furthermore, as a compound having an azole structure, a compound in which a group represented by the following formula (R-1) or the following formula (R-2) is directly bonded to the azole structure is also preferred. In formula (R-1), R 1 represents a monovalent organic group, and * represents a bonding site with the azole structure. 2 represents a hydrogen atom or a monovalent organic group, R 3 represents a monovalent organic group, and * represents a bonding site with the azole structure. 1 is a hydrocarbon group, or a hydrocarbon group and —O—, —C(═O)—, —S—, —S(═O) 2 - and -NR N - is preferably a group represented by a bond to at least one group selected from the group consisting of R N is as described above. The hydrocarbon group is preferably an aliphatic hydrocarbon group, an aromatic hydrocarbon group, or a group represented by a combination thereof. 1 The total number of carbon atoms in R is preferably 1 to 30, more preferably 2 to 25, and even more preferably 3 to 20. 1 The bonding site with the carbonyl group in formula (R-1) is a hydrocarbon group or -NR N In formula (R-1), * represents a bonding site to the azole structure, and is preferably a bonding site to a carbon atom that is a ring member of the azole structure. 2 is preferably a hydrogen atom. 2 is a monovalent organic group, R 2 represents a hydrocarbon group, or a hydrocarbon group and —O—, —C(═O)—, —S—, —S(═O) 2- and -NR N - is preferably a group represented by a bond to at least one group selected from the group consisting of R N is as described above. The hydrocarbon group is preferably an aliphatic hydrocarbon group, an aromatic hydrocarbon group, or a group represented by a combination thereof. 2 When R is a monovalent organic group, the total number of carbon atoms is preferably 1 to 30, more preferably 2 to 25, and even more preferably 3 to 20. 2 is a monovalent organic group, R 2 The bonding site to the nitrogen atom in formula (R-2) in formula (R-2) is preferably a hydrocarbon group or —C(═O)—. 3 is a hydrocarbon group, or a hydrocarbon group and —O—, —C(═O)—, —S—, —S(═O) 2 - and -NR N - is preferably a group represented by a bond to at least one group selected from the group consisting of R N is as described above. The hydrocarbon group is preferably an aliphatic hydrocarbon group, an aromatic hydrocarbon group, or a group represented by a combination thereof. 3 When R is a monovalent organic group, the total number of carbon atoms is preferably 1 to 30, more preferably 2 to 25, and even more preferably 3 to 20. 3 In formula (R-2), the bonding site to the nitrogen atom is preferably a hydrocarbon group or -C(=O)-. In formula (R-2), * represents the bonding site to the azole structure, and is preferably the bonding site to a carbon atom that is a ring member of the azole structure.
[0192] As the migration inhibitor, an ion trapping agent that traps anions such as halogen ions can also be used.
[0193] Other migration inhibitors include the rust inhibitors described in paragraph 0094 of JP-A-2013-015701, the compounds described in paragraphs 0073 to 0076 of JP-A-2009-283711, the compounds described in paragraph 0052 of JP-A-2011-059656, the compounds described in paragraphs 0114, 0116 and 0118 of JP-A-2012-194520, and the compounds described in paragraph 0166 of WO 2015 / 199219. The contents of this specification are incorporated herein by reference.
[0194] Specific examples of the migration inhibitor include the following compounds.
[0195]
[0196] When the resin composition of the present invention contains a migration inhibitor, the content of the migration inhibitor is preferably 0.01 to 5.0 mass%, more preferably 0.05 to 2.0 mass%, and even more preferably 0.1 to 1.0 mass%, based on the total solid content of the resin composition.
[0197] The migration inhibitor may be one kind or two or more kinds. When two or more kinds of migration inhibitors are used, the total amount thereof is preferably within the above range.
[0198] <Light absorber> The resin composition of the present invention preferably contains a compound (light absorber) whose absorbance at the exposure wavelength is reduced by exposure. Examples of the light absorber include the compounds described in paragraphs 0159 to 0183 of WO 2022 / 202647 and the compounds described in paragraphs 0088 to 0108 of JP 2019-206689 A. The contents of these compounds are incorporated herein by reference.
[0199] The content of the light absorber relative to the total solid content of the resin composition of the present invention is not particularly limited, but is preferably 0.1 to 20 mass%, more preferably 0.5 to 10 mass%, and even more preferably 1 to 5 mass%.
[0200] <Polymerization Inhibitor> The resin composition of the present invention preferably contains a polymerization inhibitor. Examples of the polymerization inhibitor include phenolic compounds, quinone compounds, amino compounds, N-oxyl free radical compounds, nitro compounds, nitroso compounds, heteroaromatic ring compounds, and metal compounds.
[0201] Specific examples of the polymerization inhibitor include the compounds described in paragraph 0310 of WO 2021 / 112189, p-hydroquinone, o-hydroquinone, 4-hydroxy-2,2,6,6-tetramethylpiperidine 1-oxyl free radical, phenoxazine, 1,4,4-trimethyl-2,3-diazabicyclo[3.2.2]non-2-ene-N,N-dioxide, and the like, the contents of which are incorporated herein by reference.
[0202] When the resin composition of the present invention contains a polymerization inhibitor, the content of the polymerization inhibitor is preferably 0.01 to 20 mass%, more preferably 0.02 to 15 mass%, and even more preferably 0.05 to 10 mass%, based on the total solid content of the resin composition.
[0203] The polymerization inhibitor may be one kind or two or more kinds. When two or more kinds of polymerization inhibitors are used, the total amount thereof is preferably within the above range.
[0204] <Other Additives> The resin composition of the present invention may contain various additives, as needed, within the scope of obtaining the effects of the present invention, such as surfactants, higher fatty acid derivatives, thermal polymerization initiators, inorganic particles, ultraviolet absorbers, organic titanium compounds, antioxidants, photoacid generators, anti-aggregation agents, phenolic compounds, other polymer compounds, plasticizers, and other auxiliary agents (e.g., antifoaming agents, flame retardants, etc.). By appropriately incorporating these components, it is possible to adjust properties such as film physical properties. For details of these components, please refer to, for example, the descriptions in paragraphs 0183 and after of JP 2012-003225 A (corresponding to paragraph 0237 of U.S. Patent Application Publication No. 2013 / 0034812 ), and the descriptions in paragraphs 0101 to 0104 and 0107 to 0109 of JP 2008-250074 A, the contents of which are incorporated herein by reference. When these additives are blended, the total content thereof is preferably 3% by mass or less of the solid content of the resin composition of the present invention.
[0205] [Inorganic Particles] Specific examples of inorganic particles include calcium carbonate, calcium phosphate, silica, kaolin, talc, titanium dioxide, alumina, barium sulfate, calcium fluoride, lithium fluoride, zeolite, molybdenum sulfide, and glass.
[0206] The average particle size of the inorganic particles is preferably 0.01 to 2.0 μm, more preferably 0.02 to 1.5 μm, even more preferably 0.03 to 1.0 μm, and particularly preferably 0.04 to 0.5 μm. The above average particle size of the inorganic particles is the primary particle size and also the volume average particle size. The volume average particle size can be measured, for example, by dynamic light scattering using a Nanotrac WAVE II EX-150 (manufactured by Nikkiso Co., Ltd.). If the above measurement is difficult, it can also be measured by centrifugal sedimentation light transmission method, X-ray transmission method, or laser diffraction / scattering method.
[0207] [Organotitanium Compound] When the resin composition contains an organotitanium compound, a resin layer having excellent chemical resistance can be formed even when cured at low temperatures.
[0208] Usable organic titanium compounds include those in which an organic group is bonded to a titanium atom via a covalent bond or an ionic bond. Specific examples of organic titanium compounds are shown below in I) to VII): I) Titanium chelate compounds: Titanium chelate compounds having two or more alkoxy groups are more preferred because they provide good storage stability to the resin composition and a good curing pattern. Specific examples include titanium bis(triethanolamine) diisopropoxide, titanium di(n-butoxide) bis(2,4-pentanedionate), titanium diisopropoxide bis(2,4-pentanedionate), titanium diisopropoxide bis(tetramethylheptanedionate), and titanium diisopropoxide bis(ethylacetoacetate). II) Tetraalkoxytitanium compounds: for example, titanium tetra(n-butoxide), titanium tetraethoxide, titanium tetra(2-ethylhexoxide), titanium tetraisobutoxide, titanium tetraisopropoxide, titanium tetramethoxide, titanium tetramethoxypropoxide, titanium tetramethylphenoxide, titanium tetra(n-nonyloxide), titanium tetra(n-propoxide), titanium tetrastearyloxide, titanium tetrakis[bis{2,2-(allyloxymethyl)butoxide}], etc. III) Titanocene compounds: for example, pentamethylcyclopentadienyltitanium trimethoxide, bis(η5-2,4-cyclopentadien-1-yl)bis(2,6-difluorophenyl)titanium, bis(η5-2,4-cyclopentadien-1-yl)bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium, etc. IV) Monoalkoxytitanium compounds: for example, titanium tris(dioctylphosphate)isopropoxide, titanium tris(dodecylbenzenesulfonate)isopropoxide, etc. V) Titanium oxide compounds: for example, titanium oxide bis(pentanedionate), titanium oxide bis(tetramethylheptanedionate), phthalocyanine titanium oxide, etc.VI) Titanium tetraacetylacetonate compounds: for example, titanium tetraacetylacetonate, etc. VII) Titanate coupling agents: for example, isopropyl tridodecylbenzenesulfonyl titanate, etc.
[0209] Among these, from the viewpoint of better chemical resistance, the organic titanium compound is preferably at least one compound selected from the group consisting of I) titanium chelate compounds, II) tetraalkoxytitanium compounds, and III) titanocene compounds. In particular, titanium diisopropoxide bis(ethylacetoacetate), titanium tetra(n-butoxide), and bis(η5-2,4-cyclopentadien-1-yl)bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium are preferred.
[0210] It is also preferable to contain a compound represented by the following formula (T-1) as the organotitanium compound or in place of the organotitanium compound. In formula (T-1), M is titanium, zirconium, or hafnium, l1 is an integer of 0 to 2, l2 is 0 or 1, l1 + l2 × 2 is an integer of 0 to 2, m is an integer of 0 to 4, n is an integer of 0 to 2, l1 + l2 + m + n × 2 = 4, and R 11 are each independently a substituted or unsubstituted cyclopentadienyl group, a substituted or unsubstituted alkoxy group, or a substituted or unsubstituted phenoxy group; R 12 is a substituted or unsubstituted hydrocarbon group, R 2 are each independently a group containing a structure represented by the following formula (T-2), and R 3 are each independently a group containing a structure represented by the following formula (T-2), A are each independently an oxygen atom or a sulfur atom. In formula (T-2), X 1 ~X 3 each independently represents -C(-*)= or -N=, * represents a bonding site to another structure, and # represents a bonding site to a metal atom.
[0211] In formula (T-1), from the viewpoint of storage stability of the composition, M is preferably titanium. In formula (T-1), an embodiment in which l1 and l2 are 0 is also one of the preferred embodiments of the present invention. In formula (T-1), m is preferably 2 or 4, and more preferably 2. In formula (T-1), n is preferably 1 or 2, and more preferably 1. Here, it is also preferable that in formula (T-1), l1 and l2 are 0, and m is 0, 2, or 4.
[0212] In formula (T-1), from the viewpoint of the stability of the specific metal complex, R 11 is preferably a substituted or unsubstituted cyclopentadienyl ligand. 11 The cyclopentadienyl group, alkoxy group and phenoxy group in the formula (I) may be substituted, but an embodiment in which they are unsubstituted is also one of the preferred embodiments of the present invention.
[0213] In formula (T-1), R 12 is preferably a hydrocarbon group having 1 to 20 carbon atoms, and more preferably a hydrocarbon group having 2 to 10 carbon atoms. 12 The hydrocarbon group in may be either an aliphatic hydrocarbon group or an aromatic hydrocarbon group, but an aromatic hydrocarbon group is preferred. The aliphatic hydrocarbon group may be either a saturated aliphatic hydrocarbon group or an unsaturated aliphatic hydrocarbon group, but a saturated aliphatic hydrocarbon group is preferred. The aromatic hydrocarbon group is preferably an aromatic hydrocarbon group having 6 to 20 carbon atoms, more preferably an aromatic hydrocarbon group having 6 to 10 carbon atoms, and even more preferably a phenylene group. R 12 The substituent in R is preferably a monovalent substituent, such as a halogen atom. 12 When R is an aromatic hydrocarbon group, it may have an alkyl group as a substituent. 12 is preferably an unsubstituted phenylene group. 12 The phenylene group in is preferably a 1,2-phenylene group.
[0214] In formula (T-1), m is 2 or more, and R 2 If two or more are included,2 In formula (T-1), n is 2 or more, and R 3 If two or more are included, 3 The structures may be the same or different.
[0215] In formula (T-2), X 1 ~X 3 each independently represents -C(-*)= or -N=, and it is preferable that at least one represents -C(-*)=, and it is more preferable that at least two represent -C(-*)=.
[0216] Specific examples of the compound represented by formula (T-1) include compounds I-5 to I-8 in the examples, but are not limited to these.
[0217] When an organotitanium compound is contained, its content is preferably 0.05 to 10 parts by mass, and more preferably 0.1 to 5 parts by mass, relative to 100 parts by mass of the specific resin. When the content is 0.05 part by mass or more, the heat resistance and chemical resistance of the obtained cured pattern are improved, and when it is 10 parts by mass or less, the storage stability of the composition is improved.
[0218] When an organotitanium compound is included, its content is preferably 0.05 to 10 parts by mass, and more preferably 0.1 to 2 parts by mass, per 100 parts by mass of the specific resin. When the content is 0.05 parts by mass or more, the heat resistance and chemical resistance of the resulting cured pattern are improved, and when it is 10 parts by mass or less, the storage stability of the composition is superior. Other additives include the compounds described in paragraphs 0316 to 0358 of WO 2022 / 145355. The above descriptions are incorporated herein by reference.
[0219] <Characteristics of Resin Composition> The viscosity of the resin composition of the present invention can be adjusted by the solid content concentration of the resin composition. 2 / s~12,000mm 2 / s is preferred, and 2,000 mm 2 / s~10,000mm 2 / s is more preferable, and 2,500 mm 2 / s~8,000mm 2 Within the above range, it is easy to obtain a highly uniform coating film. 2 If the thickness is more than 12,000 mm / s, it is easy to apply the coating to a thickness required for an insulating film for rewiring, for example. 2 If the viscosity is less than 1 / s, a coating film with excellent surface condition can be obtained.
[0220] <Restrictions on substances contained in the resin composition> The water content of the resin composition of the present invention is preferably less than 2.0% by mass, more preferably less than 1.5% by mass, and even more preferably less than 1.0% by mass. If it is less than 2.0%, the storage stability of the resin composition is improved. Methods for maintaining the water content include adjusting the humidity under storage conditions and reducing the porosity of the storage container during storage.
[0221] From the viewpoint of insulating properties, the metal content of the resin composition of the present invention is preferably less than 5 mass ppm (parts per million), more preferably less than 1 mass ppm, and even more preferably less than 0.5 mass ppm. Examples of metals include sodium, potassium, magnesium, calcium, iron, copper, chromium, and nickel, but metals contained as complexes of organic compounds and metals are excluded. When multiple metals are contained, the total amount of these metals is preferably within the above range.
[0222] Furthermore, examples of methods for reducing metal impurities unintentionally contained in the resin composition of the present invention include selecting raw materials with a low metal content as raw materials for constituting the resin composition of the present invention, filtering the raw materials for constituting the resin composition of the present invention, and lining the inside of the apparatus with polytetrafluoroethylene or the like to perform distillation under conditions that minimize contamination as much as possible.
[0223] Considering the use of the resin composition of the present invention as a semiconductor material, the content of halogen atoms is preferably less than 500 ppm by mass, more preferably less than 300 ppm by mass, and even more preferably less than 200 ppm by mass, from the viewpoint of wiring corrosion. In particular, those present in the form of halogen ions are preferably less than 5 ppm by mass, more preferably less than 1 ppm by mass, and even more preferably less than 0.5 ppm by mass. Examples of halogen atoms include chlorine atoms and bromine atoms. It is preferable that the total of chlorine atoms and bromine atoms, or chlorine ions and bromine ions, is within the above-mentioned range. Preferred methods for adjusting the content of halogen atoms include ion exchange treatment.
[0224] A conventionally known container can be used as a container for storing the resin composition of the present invention. For the purpose of preventing impurities from being mixed into the raw materials or the resin composition of the present invention, it is also preferable to use a multi-layer bottle whose inner wall is made of six types of six resin layers, or a bottle with a seven-layer structure made of six types of resin. Examples of such containers include the container described in JP 2015-123351 A.
[0225] <Cured Product of Resin Composition> A cured product of the resin composition can be obtained by curing the resin composition of the present invention. The cured product of the present invention is a cured product obtained by curing the resin composition. The resin composition is preferably cured by heating, with a heating temperature of 120°C to 400°C being more preferred, 140°C to 380°C being even more preferred, and 170°C to 350°C being particularly preferred. The form of the cured product of the resin composition is not particularly limited, and can be selected depending on the application, such as a film, rod, sphere, or pellet. In the present invention, the cured product is preferably in the form of a film. By patterning the resin composition, the shape of the cured product can be selected depending on the application, such as forming a protective film on a wall surface, forming via holes for electrical conductivity, adjusting impedance, capacitance, or internal stress, or imparting heat dissipation functionality. The film thickness of the cured product (film made of the cured product) is preferably 0.5 μm or more and 150 μm or less. The shrinkage rate when the resin composition of the present invention is cured is preferably 50% or less, more preferably 45% or less, and even more preferably 40% or less. Here, the shrinkage rate refers to the percentage of change in volume of the resin composition before and after curing, and can be calculated by the following formula: Shrinkage rate [%] = 100 - (volume after curing / volume before curing) x 100
[0226] <Characteristics of cured product of resin composition> The imidization reaction rate of the cured product of the resin composition of the present invention is preferably 70% or more, more preferably 80% or more, and even more preferably 90% or more. If it is 70% or more, the cured product may have excellent mechanical properties. The elongation at break of the cured product of the resin composition of the present invention is preferably 30% or more, more preferably 40% or more, and even more preferably 50% or more. The glass transition temperature (Tg) of the cured product of the resin composition of the present invention is preferably 180°C or more, more preferably 210°C or more, and even more preferably 230°C or more.
[0227] <Preparation of Resin Composition> The resin composition of the present invention can be prepared by mixing the above-mentioned components. The mixing method is not particularly limited, and can be carried out by a conventionally known method. Examples of the mixing method include mixing with a stirring blade, mixing with a ball mill, and mixing by rotating a tank. The temperature during mixing is preferably 10 to 30°C, more preferably 15 to 25°C.
[0228] Filtration using a filter is preferably performed to remove foreign matter such as dust and fine particles from the resin composition of the present invention. The filter pore size is, for example, preferably 5 μm or less, more preferably 1 μm or less, even more preferably 0.5 μm or less, and even more preferably 0.1 μm or less. The filter material is preferably polytetrafluoroethylene, polyethylene, or nylon. When the filter material is polyethylene, HDPE (high-density polyethylene) is more preferable. The filter may be pre-washed with an organic solvent. In the filter filtration process, multiple types of filters may be connected in series or parallel. When multiple types of filters are used, filters with different pore sizes or materials may be combined. An example of a connection mode is a mode in which an HDPE filter with a pore size of 1 μm is connected in series as the first stage and an HDPE filter with a pore size of 0.2 μm is connected in series as the second stage. Various materials may also be filtered multiple times. When filtration is performed multiple times, circulating filtration may be used. Filtration may also be performed under pressure. When filtering under pressure, the pressure to be applied is preferably 0.01 MPa or more and 1.0 MPa or less, more preferably 0.03 MPa or more and 0.9 MPa or less, even more preferably 0.05 MPa or more and 0.7 MPa or less, and even more preferably 0.05 MPa or more and 0.5 MPa or less. In addition to filtering using a filter, a process of removing impurities using an adsorbent may be performed. Filter filtration and a process of removing impurities using an adsorbent may be combined. Known adsorbents can be used as the adsorbent. Examples include inorganic adsorbents such as silica gel and zeolite, and organic adsorbents such as activated carbon. After filtering using a filter, the resin composition filled in a bottle may be subjected to a degassing process by placing it under reduced pressure.
[0229] (Method for producing a cured product) The method for producing a cured product of the present invention preferably includes a film-forming step in which a resin composition is applied to a substrate to form a film. The method for producing a cured product more preferably includes the film-forming step, an exposure step in which the film formed in the film-forming step is selectively exposed to light, and a development step in which the film exposed in the exposure step is developed using a developer to form a pattern. The method for producing a cured product particularly preferably includes the film-forming step, the exposure step, the development step, and at least one of a heating step in which the pattern obtained in the development step is heated and a post-development exposure step in which the pattern obtained in the development step is exposed to light. The method for producing a cured product also preferably includes the film-forming step and a step of heating the film. Details of each step are described below.
[0230] <Film Forming Step> The resin composition of the present invention can be used in a film forming step of applying the resin composition to a substrate to form a film. The method for producing a cured product of the present invention preferably includes a film forming step of applying the resin composition to a substrate to form a film.
[0231] [Substrate] The type of substrate can be appropriately determined depending on the application and is not particularly limited. Examples of substrates include semiconductor production substrates such as silicon, silicon nitride, polysilicon, silicon oxide, and amorphous silicon, quartz, glass, optical films, ceramic materials, vapor deposition films, magnetic films, reflective films, metal substrates such as Ni, Cu, Cr, and Fe (for example, substrates formed from metal and substrates on which a metal layer is formed by, for example, plating or vapor deposition), paper, SOG (Spin On Glass), TFT (Thin Film Transistor) array substrates, mold substrates, and plasma display panel (PDP) electrode plates. Substrates are particularly preferably semiconductor production substrates, with silicon substrates, Cu substrates, and mold substrates being more preferred. These substrates may have a surface layer such as an adhesion layer or an oxide layer formed by hexamethyldisilazane (HMDS) or the like. The shape of the substrate is not particularly limited and may be circular or rectangular. The size of the substrate is preferably, for example, a diameter of 100 to 450 mm, more preferably 200 to 450 mm, if it is circular. If it is rectangular, the length of the short side is preferably, for example, 100 to 1000 mm, more preferably 200 to 700 mm. As the substrate, for example, a plate-shaped, preferably a panel-shaped substrate (substrate) is used.
[0232] When a film is formed by applying a resin composition to the surface of a resin layer (for example, a layer made of a cured product) or the surface of a metal layer, the resin layer or the metal layer serves as the substrate.
[0233] Coating is preferred as a means for applying the resin composition to a substrate. Specific application methods include dip coating, air knife coating, curtain coating, wire bar coating, gravure coating, extrusion coating, spray coating, spin coating, slit coating, and inkjet coating. From the viewpoint of uniformity of film thickness, spin coating, slit coating, spray coating, or inkjet coating is preferred, and from the viewpoint of uniformity of film thickness and productivity, spin coating and slit coating are more preferred. By adjusting the solid content concentration of the resin composition and coating conditions depending on the application method, a film of the desired thickness can be obtained. In addition, the coating method can be appropriately selected depending on the shape of the substrate. For circular substrates such as wafers, spin coating, spray coating, inkjet coating, etc. are preferred, and for rectangular substrates, slit coating, spray coating, inkjet coating, etc. are preferred. In the case of spin coating, for example, it can be applied at a rotation speed of 500 to 3,500 rpm for about 10 seconds to 3 minutes. Alternatively, a method can be used in which a coating film formed by applying the coating composition to a temporary support using the above-described application method is transferred onto the substrate. Regarding the transfer method, the preparation methods described in paragraphs 0023 and 0036 to 0051 of JP-A No. 2006-023696 and paragraphs 0096 to 0108 of JP-A No. 2006-047592 can be suitably used. A step of removing excess film from the edge of the substrate may also be performed. Examples of such a step include edge bead rinsing (EBR) and back rinsing. A pre-wetting step may also be employed in which various solvents are applied to the substrate before applying the resin composition to improve the wettability of the substrate.
[0234] <Drying Step> After the film-forming step (layer-forming step), the film may be subjected to a step (drying step) of drying the formed film (layer) to remove the solvent. That is, the method for producing a cured product of the present invention may include a drying step of drying the film formed in the film-forming step. The drying step is preferably carried out after the film-forming step and before the exposure step. The drying temperature of the film in the drying step is preferably 50 to 150°C, more preferably 70 to 130°C, and even more preferably 90 to 110°C. Drying may also be carried out under reduced pressure. The drying time is, for example, 30 seconds to 20 minutes, preferably 1 to 10 minutes, and more preferably 2 to 7 minutes.
[0235] <Exposure Step> The film may be subjected to an exposure step in which the film is selectively exposed to light. The method for producing a cured product may include an exposure step in which the film formed in the film formation step is selectively exposed to light. Selective exposure means that a portion of the film is exposed to light. Furthermore, selective exposure forms exposed regions (exposed portions) and unexposed regions (unexposed portions) in the film. The exposure dose is not particularly limited as long as it can cure the resin composition of the present invention, but for example, it is 50 to 10,000 mJ / cm2 in terms of exposure energy at a wavelength of 365 nm. 2 is preferred, and 200 to 8,000 mJ / cm 2 is more preferred.
[0236] The exposure wavelength can be appropriately determined within the range of 190 to 1,000 nm, and is preferably 240 to 550 nm.
[0237] The exposure wavelengths, in relation to the light source, are: (1) semiconductor laser (wavelengths 830 nm, 532 nm, 488 nm, 405 nm, 375 nm, 355 nm, etc.); (2) metal halide lamp; (3) high-pressure mercury lamp, g-line (wavelength 436 nm), h-line (wavelength 405 nm), i-line (wavelength 365 nm), broad (three wavelengths of g, h, and i-line); (4) excimer laser, KrF excimer laser (wavelength 248 nm), ArF excimer laser (wavelength 193 nm), F 2Examples of such light include excimer laser (wavelength 157 nm), (5) extreme ultraviolet light; EUV (wavelength 13.6 nm), (6) electron beam, and (7) YAG laser second harmonic 532 nm and third harmonic 355 nm. For the resin composition of the present invention, exposure with a high-pressure mercury lamp is particularly preferred, and exposure with i-line is more preferred from the viewpoint of exposure sensitivity. The exposure method is not particularly limited as long as it is a method that exposes at least a portion of the film made of the resin composition of the present invention, and examples thereof include exposure using a photomask and exposure by laser direct imaging.
[0238] <Post-Exposure Bake Step> The film may be subjected to a heating step (post-exposure bake step) after exposure. That is, the method for producing a cured product of the present invention may include a post-exposure bake step in which the film exposed in the exposure step is heated. The post-exposure bake step can be carried out after the exposure step and before the development step. The heating temperature in the post-exposure bake step is preferably 50°C to 140°C, more preferably 60°C to 120°C. The heating time in the post-exposure bake step is preferably 30 seconds to 300 minutes, more preferably 1 minute to 10 minutes. The temperature rise rate in the post-exposure bake step from the temperature at the start of heating to the maximum heating temperature is preferably 1 to 12°C / min, more preferably 2 to 10°C / min, and even more preferably 3 to 10°C / min. The temperature rise rate may also be changed as appropriate during heating. The heating means in the post-exposure bake step is not particularly limited, and known hot plates, ovens, infrared heaters, etc. may be used. It is also preferable to carry out the heating in an atmosphere of low oxygen concentration by flowing an inert gas such as nitrogen, helium, or argon.
[0239] <Development step> The above-mentioned film after exposure may be subjected to a development step in which it is developed using a developer to form a pattern. That is, the method for producing a cured product of the present invention may include a development step in which the film exposed in the exposure step is developed using a developer to form a pattern. By carrying out development, one of the exposed and unexposed parts of the film is removed to form a pattern. Here, development in which the unexposed parts of the film are removed in the development step is called negative development, and development in which the exposed parts of the film are removed in the development step is called positive development.
[0240] [Developer] The developer used in the development step may be an aqueous alkaline solution or a developer containing an organic solvent.
[0241] When the developer is an alkaline aqueous solution, examples of the basic compound that can be contained in the alkaline aqueous solution include inorganic alkalis, primary amines, secondary amines, tertiary amines, and quaternary ammonium salts. Preferred are TMAH (tetramethylammonium hydroxide), potassium hydroxide, sodium carbonate, sodium hydroxide, sodium silicate, sodium metasilicate, ammonia, ethylamine, n-propylamine, diethylamine, di-n-butylamine, triethylamine, methyldiethylamine, dimethylethanolamine, triethanolamine, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, tetrapentylammonium hydroxide, tetrahexylammonium hydroxide, tetraoctylammonium hydroxide, ethyltrimethylammonium hydroxide, butyltrimethylammonium hydroxide, methyltriamylammonium hydroxide, dibutyldipentylammonium hydroxide, dimethylbis(2-hydroxyethyl)ammonium hydroxide, trimethylphenylammonium hydroxide, trimethylbenzylammonium hydroxide, triethylbenzylammonium hydroxide, pyrrole, and piperidine, and more preferred is TMAH. The content of the basic compound in the developer is preferably from 0.01 to 10% by mass, more preferably from 0.1 to 5% by mass, and even more preferably from 0.3 to 3% by mass, based on the total mass of the developer.
[0242] When the developer contains an organic solvent, the organic solvent may be a compound described in paragraph
[0387] of WO 2021 / 112189, the contents of which are incorporated herein by reference. Suitable examples of alcohols include methanol, ethanol, propanol, isopropanol, butanol, pentanol, octanol, diethylene glycol, propylene glycol, methyl isobutyl carbinol, and triethylene glycol, and suitable examples of amides include N-methylpyrrolidone, N-ethylpyrrolidone, and dimethylformamide.
[0243] When the developer contains an organic solvent, the organic solvent may be used alone or in combination. In the present invention, a developer containing at least one selected from the group consisting of cyclopentanone, γ-butyrolactone, dimethyl sulfoxide, N-methyl-2-pyrrolidone, and cyclohexanone is particularly preferred, a developer containing at least one selected from the group consisting of cyclopentanone, γ-butyrolactone, and dimethyl sulfoxide is more preferred, and a developer containing cyclopentanone is particularly preferred.
[0244] When the developer contains an organic solvent, the content of the organic solvent relative to the total mass of the developer is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more. Alternatively, the content may be 100% by mass.
[0245] The developer may further contain other components, such as known surfactants and known defoaming agents.
[0246] [Method of Supplying Developer] The method of supplying the developer is not particularly limited as long as it can form the desired pattern, and includes a method of immersing a substrate on which a film has been formed in the developer, puddle development in which the developer is supplied to the film formed on the substrate using a nozzle, and a method of continuously supplying the developer. The type of nozzle is not particularly limited, and examples include a straight nozzle, a shower nozzle, and a spray nozzle. From the viewpoints of the permeability of the developer, the removability of non-image areas, and production efficiency, a method of supplying the developer using a straight nozzle or a method of continuously supplying the developer using a spray nozzle is preferred, and from the viewpoint of the permeability of the developer to the image areas, a method of supplying using a spray nozzle is more preferred. In addition, a process may be adopted in which the developer is continuously supplied using a straight nozzle, the substrate is spun to remove the developer from the substrate, and after spin drying, the developer is continuously supplied again using a straight nozzle, and the substrate is spun to remove the developer from the substrate, or this process may be repeated multiple times. Methods of supplying the developer in the development process include a process in which the developer is continuously supplied to the substrate, a process in which the developer is kept substantially stationary on the substrate, a process in which the developer is vibrated on the substrate using ultrasound or the like, and a combination thereof.
[0247] The development time is preferably 10 seconds to 10 minutes, more preferably 20 seconds to 5 minutes. The temperature of the developer during development is not particularly limited, but is preferably 10 to 45°C, more preferably 18 to 30°C.
[0248] In the developing step, after the treatment with the developer, the pattern may be further washed (rinsed) with a rinse liquid. Alternatively, a method may be employed in which a rinse liquid is supplied before the developer in contact with the pattern is completely dried.
[0249] [Rinse Liquid] When the developer is an alkaline aqueous solution, for example, water can be used as the rinse liquid. When the developer is a developer containing an organic solvent, for example, a solvent different from the solvent contained in the developer (for example, water, an organic solvent different from the organic solvent contained in the developer) can be used as the rinse liquid.
[0250] When the rinse solution contains an organic solvent, examples of the organic solvent include the same organic solvents as those exemplified when the developer contains an organic solvent. The organic solvent contained in the rinse solution is preferably different from the organic solvent contained in the developer, and more preferably an organic solvent that has a lower solubility for the pattern than the organic solvent contained in the developer.
[0251] When the rinse solution contains an organic solvent, the organic solvent may be used alone or in combination of two or more. The organic solvent is preferably cyclopentanone, γ-butyrolactone, dimethyl sulfoxide, N-methylpyrrolidone, cyclohexanone, PGMEA, or PGME, more preferably cyclopentanone, γ-butyrolactone, dimethyl sulfoxide, PGMEA, or PGME, and even more preferably cyclohexanone or PGMEA.
[0252] When the rinse solution contains an organic solvent, the organic solvent preferably accounts for 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more of the total mass of the rinse solution, and may also account for 100% by mass of the total mass of the rinse solution.
[0253] The rinse liquid may further contain other components, such as known surfactants and known defoaming agents.
[0254] [Method of Supplying Rinse Liquid] The method of supplying the rinse liquid is not particularly limited as long as it can form a desired pattern, and examples thereof include a method of immersing the substrate in the rinse liquid, a method of supplying the rinse liquid to the substrate by puddling, a method of supplying the rinse liquid to the substrate by showering, and a method of continuously supplying the rinse liquid onto the substrate by means of a straight nozzle or the like. From the viewpoints of the permeability of the rinse liquid, the removability of non-image areas, and production efficiency, methods of supplying the rinse liquid using a shower nozzle, straight nozzle, spray nozzle, etc. are available, and a method of continuously supplying using a spray nozzle is preferred, and from the viewpoint of the permeability of the rinse liquid into the image areas, a method of supplying using a spray nozzle is more preferred. The type of nozzle is not particularly limited, and examples include a straight nozzle, shower nozzle, spray nozzle, etc. That is, the rinsing step is preferably a step of supplying or continuously supplying the rinse liquid to the exposed film using a straight nozzle, and more preferably a step of supplying the rinse liquid using a spray nozzle. The method of supplying the rinse liquid in the rinsing step may include a step of continuously supplying the rinse liquid to the substrate, a step of keeping the rinse liquid substantially stationary on the substrate, a step of vibrating the rinse liquid on the substrate by ultrasonic waves or the like, and a combination of these steps.
[0255] The rinsing time is preferably 10 seconds to 10 minutes, more preferably 20 seconds to 5 minutes. The temperature of the rinsing liquid during rinsing is not particularly limited, but is preferably 10 to 45°C, more preferably 18 to 30°C.
[0256] <Heating Step> The pattern obtained in the development step (or the pattern after rinsing, if a rinsing step is performed) may be subjected to a heating step in which the pattern obtained by the development step is heated. That is, the method for producing a cured product of the present invention may include a heating step in which the pattern obtained in the development step is heated. Alternatively, the method for producing a cured product of the present invention may include a heating step in which a pattern obtained by another method without performing a development step, or a film obtained in the film formation step, is heated. In the heating step, a resin such as a polyimide precursor is cyclized to form a resin such as a polyimide. Furthermore, crosslinking of unreacted crosslinkable groups in the specific resin or in a polymerizable compound other than the specific resin also proceeds. The heating temperature (maximum heating temperature) in the heating step is preferably 50 to 450°C, more preferably 150 to 350°C, even more preferably 150 to 250°C, even more preferably 160 to 250°C, and particularly preferably 160 to 230°C.
[0257] The heating step is preferably a step in which the cyclization reaction of the polyimide precursor is promoted within the pattern by the action of a base or the like generated from the base generator due to heating.
[0258] The heating step is preferably carried out at a temperature increase rate of 1 to 12°C / min from the temperature at the start of heating to the maximum heating temperature. The temperature increase rate is more preferably 2 to 10°C / min, and even more preferably 3 to 10°C / min. By setting the temperature increase rate to 1°C / min or more, it is possible to prevent excessive volatilization of the acid or solvent while ensuring productivity, and by setting the temperature increase rate to 12°C / min or less, it is possible to alleviate residual stress in the cured product. In addition, in the case of an oven capable of rapid heating, it is preferable to increase the temperature from the temperature at the start of heating to the maximum heating temperature at a temperature increase rate of 1 to 8°C / sec, more preferably 2 to 7°C / sec, and even more preferably 3 to 6°C / sec.
[0259] The temperature at the start of heating is preferably 20°C to 150°C, more preferably 20°C to 130°C, and even more preferably 25°C to 120°C. The temperature at the start of heating refers to the temperature at the start of the process of heating up to the maximum heating temperature. For example, when the resin composition of the present invention is applied to a substrate and then dried, the temperature is the temperature of the film (layer) after this drying, and it is preferable to raise the temperature from, for example, a temperature 30 to 200°C lower than the boiling point of the solvent contained in the resin composition.
[0260] The heating time (heating time at the maximum heating temperature) is preferably from 5 to 360 minutes, more preferably from 10 to 300 minutes, and even more preferably from 15 to 240 minutes.
[0261] In particular, when forming a multilayer laminate, from the viewpoint of interlayer adhesion, the heating temperature is preferably 30° C. or higher, more preferably 80° C. or higher, even more preferably 100° C. or higher, and particularly preferably 120° C. or higher. The upper limit of the heating temperature is preferably 350° C. or lower, more preferably 250° C. or lower, and even more preferably 240° C. or lower.
[0262] Heating may be performed in stages. For example, the temperature may be increased from 25°C to 120°C at a rate of 3°C / min, held at 120°C for 60 minutes, increased from 120°C to 180°C at a rate of 2°C / min, and held at 180°C for 120 minutes. It is also preferable to treat the film while irradiating it with ultraviolet light, as described in U.S. Pat. No. 9,159,547. Such a pretreatment step can improve the film's properties. The pretreatment step may be performed for a short period of time, preferably from 10 seconds to 2 hours, more preferably from 15 seconds to 30 minutes. The pretreatment step may be performed in two or more steps. For example, a first pretreatment step may be performed in the range of 100 to 150°C, followed by a second pretreatment step in the range of 150 to 200°C. Furthermore, cooling may be performed after heating. In this case, the cooling rate is preferably from 1 to 5°C / min.
[0263] The heating step is preferably carried out in an atmosphere with a low oxygen concentration by flowing an inert gas such as nitrogen, helium, or argon, or by carrying out the heating step under reduced pressure, in order to prevent decomposition of the specific resin. The oxygen concentration is preferably 50 ppm (volume ratio) or less, more preferably 20 ppm (volume ratio) or less. The heating means used in the heating step is not particularly limited, and examples thereof include a hot plate, an infrared oven, an electric heating oven, a hot air oven, and an infrared oven.
[0264] <Post-development exposure step> The pattern obtained in the development step (if a rinsing step is performed, the pattern after rinsing) may be subjected to a post-development exposure step in which the pattern obtained in the development step is exposed to light, instead of or in addition to the heating step. That is, the method for producing a cured product of the present invention may include a post-development exposure step in which the pattern obtained in the development step is exposed to light. The method for producing a cured product of the present invention may include a heating step and a post-development exposure step, or may include only one of the heating step and the post-development exposure step. The post-development exposure step can promote, for example, a reaction in which cyclization of a polyimide precursor or the like progresses due to exposure of a photobase generator, or a reaction in which elimination of an acid-decomposable group progresses due to exposure of a photoacid generator. In the post-development exposure step, it is sufficient that at least a portion of the pattern obtained in the development step is exposed, but it is preferable that the entire pattern is exposed. The exposure dose in the post-development exposure step is 50 to 20,000 mJ / cm in terms of exposure energy at a wavelength to which the photosensitive compound has sensitivity. 2 is preferred, and 100 to 15,000 mJ / cm 2 The post-development exposure step can be carried out using, for example, the light source used in the exposure step described above, and it is preferable to use broadband light.
[0265] <Metal Layer Forming Step> The pattern obtained by the developing step (preferably subjected to at least one of a heating step and a post-development exposure step) may be subjected to a metal layer forming step of forming a metal layer on the pattern. That is, the method for producing a cured product of the present invention preferably includes a metal layer forming step of forming a metal layer on the pattern obtained by the developing step (preferably subjected to at least one of a heating step and a post-development exposure step).
[0266] The metal layer is not particularly limited, and existing metal species can be used. Examples include copper, aluminum, nickel, vanadium, titanium, chromium, cobalt, gold, tungsten, tin, silver, and alloys containing these metals. Copper and aluminum are more preferred, and copper is even more preferred.
[0267] The method for forming the metal layer is not particularly limited, and existing methods can be applied. For example, the methods described in JP 2007-157879 A, JP 2001-521288 A, JP 2004-214501 A, JP 2004-101850 A, U.S. Patent No. 7,888,181 B2, and U.S. Patent No. 9,177,926 B2 can be used. Examples of suitable methods include photolithography, PVD (physical vapor deposition), CVD (chemical vapor deposition), lift-off, electroplating, electroless plating, etching, printing, and combinations of these. More specifically, examples include patterning methods that combine sputtering, photolithography, and etching, and patterning methods that combine photolithography and electroplating. Preferred plating methods include electroplating using a copper sulfate or copper cyanide plating solution.
[0268] The thickness of the metal layer is preferably 0.01 to 50 μm, more preferably 1 to 10 μm, at the thickest part.
[0269] <Applications> Fields to which the method for producing a cured product of the present invention or the cured product can be applied include insulating films for electronic devices, interlayer insulating films for rewiring layers, stress buffer films, etc. Other examples include sealing films, substrate materials (base films, coverlays, and interlayer insulating films for flexible printed circuit boards), and the etching of insulating films for packaging applications such as those described above. For these applications, reference can be made to, for example, Science & Technology Co., Ltd.'s "High Performance Polyimide and Application Technology" (April 2008), edited by Masaaki Kakimoto, CMC Technical Library "Fundamentals and Development of Polyimide Materials" (November 2011), and Japan Polyimide and Aromatic Polymer Research Association's "Latest Polyimide Fundamentals and Applications" (NTS, August 2010).
[0270] The method for producing the cured product of the present invention, or the cured product of the present invention, can also be used for producing printing plates such as offset printing plates or screen printing plates, for etching molded parts, for producing protective lacquers and dielectric layers in electronics, especially microelectronics, etc.
[0271] (Laminate and method for manufacturing laminate) The laminate of the present invention refers to a structure having a plurality of layers each made of the cured product of the present invention. The laminate is a laminate including two or more layers each made of the cured product, and may be a laminate including three or more layers. At least one of the two or more layers each made of the cured product contained in the laminate is a layer made of the cured product of the present invention, and from the viewpoint of suppressing shrinkage of the cured product or deformation of the cured product associated with the shrinkage, it is also preferable that all of the layers made of the cured product contained in the laminate are layers made of the cured product of the present invention.
[0272] That is, the method for producing a laminate of the present invention preferably includes the method for producing a cured product of the present invention, and more preferably includes repeating the method for producing a cured product of the present invention multiple times.
[0273] The laminate of the present invention preferably includes two or more layers made of a cured product and a metal layer between any of the layers made of the cured product. The metal layer is preferably formed by the metal layer-forming step. That is, the method for producing a laminate of the present invention preferably further includes a metal layer-forming step of forming a metal layer on a layer made of a cured product between multiple cured product production processes. A preferred embodiment of the metal layer-forming step is as described above. Examples of the laminate include a laminate having at least a layer structure in which three layers are stacked in this order: a layer made of a first cured product, a metal layer, and a layer made of a second cured product. It is preferred that both the layer made of the first cured product and the layer made of the second cured product are layers made of the cured product of the present invention. The resin composition of the present invention used to form the layer made of the first cured product and the resin composition of the present invention used to form the layer made of the second cured product may have the same composition or different compositions. The metal layer in the laminate of the present invention is preferably used as metal wiring, such as a rewiring layer.
[0274] <Lamination Step> The method for producing a laminate of the present invention preferably includes a lamination step. The lamination step is a series of steps including performing at least one of (a) a film formation step (layer formation step), (b) an exposure step, (c) a development step, and (d) a heating step and a post-development exposure step again on the surface of the pattern (resin layer) or the metal layer in this order. However, at least one of (a) the film formation step and (d) the heating step and the post-development exposure step may be repeated. Furthermore, after at least one of (d) the heating step and the post-development exposure step, (e) a metal layer formation step may be included. It goes without saying that the lamination step may further include the above-mentioned drying step or the like as appropriate.
[0275] When a further lamination step is performed after the lamination step, a surface activation treatment step may be further performed after the exposure step, the heating step, or the metal layer forming step. An example of the surface activation treatment is a plasma treatment. Details of the surface activation treatment will be described later.
[0276] The lamination step is preferably performed 2 to 20 times, more preferably 2 to 9 times. For example, a structure having 2 to 20 resin layers, such as resin layer / metal layer / resin layer / metal layer / resin layer / metal layer, is preferred, and a structure having 2 to 9 resin layers is even more preferred. Each of the layers may be the same or different in composition, shape, film thickness, etc.
[0277] In the present invention, a particularly preferred embodiment is one in which, after providing a metal layer, a cured product (resin layer) of the resin composition of the present invention is further formed so as to cover the metal layer.Specific examples include an embodiment in which the steps of (a) film formation step, (b) exposure step, (c) development step, (d) at least one of a heating step and a post-development exposure step, and (e) metal layer formation step are repeated in this order, or an embodiment in which the steps of (a) film formation step, (d) at least one of a heating step and a post-development exposure step, and (e) metal layer formation step are repeated in this order.By alternately performing the lamination step of laminating the resin composition layer (resin layer) of the present invention and the metal layer formation step, the resin composition layer (resin layer) of the present invention and the metal layer can be alternately laminated.
[0278] (Surface Activation Treatment Step) The method for producing a laminate of the present invention preferably includes a surface activation treatment step in which at least a portion of the metal layer and the resin composition layer are surface-activated. The surface activation treatment step is usually performed after the metal layer formation step, but after the development step (preferably after at least one of the heating step and the post-development exposure step), the resin composition layer may be surface-activated before the metal layer formation step. The surface activation treatment may be performed only on at least a portion of the metal layer, or only on at least a portion of the resin composition layer after exposure, or may be performed on at least a portion of both the metal layer and the resin composition layer after exposure. The surface activation treatment is preferably performed on at least a portion of the metal layer, and it is preferable to perform the surface activation treatment on part or all of the region of the metal layer on which the resin composition layer is to be formed. In this way, by performing the surface activation treatment on the surface of the metal layer, adhesion with the resin composition layer (film) provided on the surface can be improved. The surface activation treatment is also preferably performed on part or all of the resin composition layer (resin layer) after exposure. In this way, by performing the surface activation treatment on the surface of the resin composition layer, adhesion with the metal layer or resin layer provided on the surface that has been surface-activated can be improved. In particular, when negative development is performed, when the resin composition layer is cured, it is less susceptible to damage due to surface treatment and adhesion is likely to be improved. The surface activation treatment can be carried out, for example, by the method described in paragraph 0415 of International Publication No. 2021 / 112189. The contents of this specification are incorporated herein.
[0279] (Semiconductor device and manufacturing method thereof) The present invention also discloses a semiconductor device comprising the cured product or laminate of the present invention. The present invention also discloses a manufacturing method for a semiconductor device comprising the manufacturing method for the cured product or the manufacturing method for the laminate of the present invention. Specific examples of semiconductor devices using the resin composition of the present invention to form an interlayer insulating film for a rewiring layer can be found in paragraphs 0213 to 0218 and FIG. 1 of JP 2016-027357 A, the contents of which are incorporated herein by reference.
[0280] (Diamine Compound) The diamine compound of the present invention is a compound represented by the following formula (4-1). In formula (4-1), R 3 and R 4 each independently represents a group having an ethylenically unsaturated bond, R 3 and R 4 At least one of the groups has an aromatic hydrocarbon group, and L is a single bond, -C(CH 3 ) 2 - or - C(CF 3 ) 2 Represents -.
[0281] In formula (4-1), R 3 and R 4 A preferred embodiment of the formula (2-1) is R 1 and R 2 Among these, in the formula (4-1), R 3 and R 4 Each of these preferably independently has a vinylphenyl group.
[0282] The diamine of the present invention can be obtained, for example, by reacting a diamine having a phenolic hydroxyl group represented by the following formula (4-C) with a compound that contains a group having an ethylenically unsaturated bond and reacts with a phenolic hydroxyl group, such as a benzyl halide substituted with a group having an ethylenically unsaturated bond, an isocyanate compound containing a group having an ethylenically unsaturated bond, etc. However, the synthesis method is not limited as long as it can produce a compound having a structure represented by the above formula (4-1). In formula (4-C), L has the same meaning as L in formula (4-1) above, and preferred embodiments are also the same.
[0283] The present invention will be explained in more detail below with reference to examples. The materials, amounts used, ratios, processing details, processing procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the specific examples shown below. Unless otherwise specified, "parts" and "%" are based on mass.
[0284] (Synthesis of Monomer) <Synthesis Example AA-1> 48.65 g (225 mmol) of 3,3'-dihydroxybenzidine and 375 mL of dimethylformamide were mixed in a 1 L flask. Under ice cooling, 98.21 g (450 mmol) of di-t-butyl dicarbonate was added dropwise. After the completion of the dropwise addition, the mixture was stirred at 60°C for 5 hours. After the reaction was completed and the mixture was cooled to room temperature, 35 mg of 2,2,6,6-tetramethylpiperidine 1-oxyl free radical, 68.68 g (450 mmol) of p-chloromethylstyrene, 74.63 g (540 mmol) of potassium carbonate, and 8.96 g (54.0 mmol) of potassium iodide were added, and the mixture was stirred at 60°C for 3 hours. After the reaction was completed, filtration was performed by suction filtration, and the filtrate was added dropwise to 500 mL of water. White crystals precipitated, and the precipitated solid was collected by suction filtration. The obtained white solid was purified by recrystallization using 1000 mL of acetone at 60°C. 125 g (yield 85.6%) of the following intermediate AA-1a was obtained. The structure of AA-1a is shown below. 1 This was confirmed by H-NMR spectrum. 1 H-NMR (BRUKER, AVANCE NEO 400): δ(ppm,DMSO-d6)8.04-7.94(s,2H), 7.75-7.64(d,2H), 7.56-7.42(m,8H), 7.27-7.20(d,2H), 7.19-7.12(d,2H), 6.79-6.64(2H), 5.89-5.77(2H), 5.30-5.15(6H), 1.49-1.43(s,18H)
[0285] 75.0 g (115.6 mmol) of (AA-1a) and 500 mL of methylene chloride were mixed in a 1 L flask. 131.8 g (1156 mmol) of trifluoroacetic acid was added at room temperature, and then the mixture was stirred at 40°C for 5 hours. After the reaction was completed, 250 mL of methanol was added dropwise under ice cooling, followed by 117.0 g (1156 mmol) of triethylamine. Pale yellow crystals were precipitated, and the precipitated solid was collected by suction filtration. The mixture was suspended and washed in 750 mL of methanol, yielding 40.5 g (73% yield) of (AA-1). The structure of AA-1 is shown below. The following structure is 1 This was confirmed by H-NMR spectrum.1 H-NMR (BRUKER, AVANCE NEO 400): δ(ppm,DMSO-d6)7.53-7.45(s,8H), 7.05-6.98(d,2H), 6.92-6.85(d,2H), 6.79-6.63(4H), 5.89-5.78(d,2H), 5.29-5.22(d,2H), 5.20-5.13(s,4H), 4.92-4.64(4H)
[0286] <Synthesis Examples AA-2, AA-3, AA-4, AA-6, AA-7> AA-2, AA-3, AA-4, AA-6, and AA-7 were obtained in the same manner as in Synthesis Example AA-1, except that 3,3'-dihydroxybenzidine was appropriately replaced. The structures of each compound are shown below. 1 This was confirmed by H-NMR spectrum.
[0287] Synthesis Example AA-5 AA-5 was obtained in the same manner as in Synthesis Example AA-1, except that p-chloromethylstyrene was replaced with Karenz MOI (manufactured by Showa Denko K.K.). The structure of AA-5 is shown below. 1 This was confirmed by H-NMR spectrum.
[0288] Synthesis Example AT-1 AT-1 was obtained in the same manner as in Synthesis Example AA-1, except that 3,3'-dihydroxybenzidine was replaced with p-methoxyphenol. The structure of AT-1 is shown below. 1 This was confirmed by H-NMR spectrum. 1 H-NMR (BRUKER, AVANCE NEO 400): δ(ppm,DMSO-d6)7.52-7.42(d,2H), 7.42-7.32(d,2H), 6.80-6.63(3H), 6.54-6.43(d,2H), 5.92-5.77(1H), 5.30-5.19(1H), 4.95-4.89(s,2H), 4.68-4.54(2H)
[0289] (Synthesis of Polymer) <Synthesis Example A-1: Synthesis of Polyimide (A-1)> 30.0 g (57.64 mmol) of 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride and 0.08 g of 2,2,6,6-tetramethylpiperidine 1-oxyl free radical were dissolved in 120 g of N-methylpyrrolidone (NMP) to obtain a solution. Next, 9.93 g (24.2 mmol) of 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 10.86 g (24.2 mmol) of AA-1, and 1.30 g (5.76 mmol) of AT-1 were dissolved in 100 g of NMP and added dropwise to the above solution over 1 hour at a temperature of 0 to 10 °C. After stirring at 25 °C for 60 minutes, 18.2 g of pyridine and 14.7 g of acetic anhydride were added and reacted at 80 °C for 4 hours. After completion of the reaction, the mixture was cooled to 25 °C and diluted with 200 g of tetrahydrofuran. Next, the reaction solution was added dropwise to a mixture of 2.0 L of methanol and 0.5 L of water, stirred for 15 minutes, and then the polyimide resin was filtered. Next, the resin was reslurried in 1 L of water, filtered, and then reslurried again in 1 L of methanol, filtered, and dried under reduced pressure at 40 °C for 10 hours. Next, the dried resin was dissolved in 250 g of tetrahydrofuran, and 40 g of ion exchange resin (MB-1: manufactured by Organo Corporation) was added thereto. The mixture was stirred for 4 hours. The ion exchange resin was removed by filtration, and then the polyimide resin was precipitated in 2 liters of methanol and stirred for 15 minutes. The polyimide resin was collected by filtration and dried at 45°C under reduced pressure for 1 day to obtain polyimide resin (A-1). The weight average molecular weight of the obtained polyimide (A-1) was 25,000 and the number average molecular weight was 9,960. Polyimide (A-1) is a resin having a repeating unit represented by the following formula (A-1). The structure of the repeating unit is: 1 The phenolic hydroxyl value (content of phenolic hydroxyl groups) of A-1 was 0.010 mmol / g, and ΔIm was 2.1%.
[0290] The phenolic hydroxyl value was calculated under the following measurement conditions: 1H-NMR (BRUKER, AVANCE NEO 400) Analysis software: TopSpin 4.0.7 Solvent: DMSO-d6 Internal standard: 1,3,5-trimethoxybenzene 1 In H-NMR, a specific peak was detected for the proton of the phenolic hydroxyl group at δ(DMSO-d6) = 10 ppm, and a specific peak was detected for the internal standard 1,3,5-trimethoxybenzene at 6.1 ppm.
[0291] ΔIm is the rate of change in imide group value before and after heating at 350°C under 1 atmosphere for 1 hour, calculated by the following formula: Rate of change (ΔIm, %) = (Im2 - Im1) × 100 / Im1 Im1: imide group value (mmol / g) before heating Im2: imide group value (mmol / g) after heating at 350°C under 1 atmosphere for 1 hour Specifically, the infrared absorption spectrum of the specific resin is measured, and the absorption peak at 1377 cm -1 Next, the specific resin was heat-treated at 350°C and 1 atmosphere for 1 hour, and then the infrared absorption spectrum was measured again. -1 The peak intensity P2 around the peak intensity P1 was determined. Using the obtained peak intensities P1 and P2, the rate of change in imide value was calculated based on the following formula. Peak intensity P1 is an index showing the imide value Im1 before heating, and peak intensity P2 is an index showing the imide value Im2 after heating. Rate of change in imide value (%) = (peak intensity P2 - peak intensity P1) x 100 / peak intensity P1
[0292] Synthesis Example A-2: Synthesis of Polyimides (A-2 to 15) Polyimides (A-2) to (A-15) were synthesized in the same manner as for polyimide (A-1), except that the raw materials used were changed appropriately. Polyimides (A-2) to (A-15) are resins having repeating units represented by the following formulas (A-2) to (A-15), respectively. The structure of each repeating unit is: 1 The molecular weights were determined from H-NMR spectra. In the structures below, the ratios indicate the molar ratios of each structure. The weight-average molecular weights and number-average molecular weights of these resins are shown in the table below.
[0293]
[0294] Synthesis Example A-16: Synthesis of Polyimide (A-16) Polyimide (A-16) was synthesized in the same manner as for polyimide (A-1), except that 10.86 g (24.2 mmol) of AA-1 in Synthesis Example 1 was replaced with a mixture of 10.32 g (23.0 mmol) of AA-1 and 0.26 g (1.2 mmol) of 3,3'-dihydroxybenzidine. The weight-average molecular weight of the resulting polyimide (A-16) was 23,000 and the number-average molecular weight was 9,150. The phenolic hydroxyl value was 0.230 mmol / g, and ΔIm was 2.0%.
[0295] Synthesis Examples A-17 and A-18: Synthesis of Polyimides (A-17 and A-18) Polyimides (A-17) and (A-18) were synthesized in the same manner as for polyimide (A-1), except that 18.2 g of pyridine and 14.7 g of acetic anhydride were added and the reaction time was changed from 4 hours in Synthesis Example 1 to 1 hour (A-17) or 2 hours (A-18). The resulting polyimide (A-17) had a weight-average molecular weight of 23,300, a number-average molecular weight of 9,250, a phenolic hydroxyl value of 0.015 mmol / g, and a ΔIm of 25.5%. The resulting polyimide (A-18) had a weight-average molecular weight of 24,700, a number-average molecular weight of 9,850, a phenolic hydroxyl value of 0.010 mmol / g, and a ΔIm of 20.7%.
[0296] Comparative Synthesis Example AC-1: Synthesis of Polyimide (AC-1) 24.74 g (40 mmol) of 4-[4-(1,3-dioxoisobenzofuran-5-ylcarbonyloxy)-2,3,5-trimethylphenyl]-2,3,6-trimethylphenyl 1,3-dioxoisobenzofuran-5-carboxylate was dissolved in 70 g of N-methylpyrrolidone (NMP) to obtain a solution. Next, 6.45 g (17.6 mmol) of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane and 5.64 g (17.6 mmol) of 4,4'-diamino-2,2'-bis(trifluoromethyl)biphenyl were dissolved in 50 g of NMP and added dropwise to the above solution at a temperature of 10 to 25°C over 1 hour. After stirring at 25°C for 30 minutes, 10 g of toluene was added, and the mixture was reacted at 200°C for 4 hours under a nitrogen flow and cooled to 25°C. Next, 4.97 g (35.2 mmol) of 2-isocyanatoethyl acrylate and 0.08 g of 2,2,6,6-tetramethylpiperidine 1-oxyl free radical were added, and the mixture was reacted at 95°C for 15 hours, cooled to 25°C, and diluted with 120 g of tetrahydrofuran. Subsequently, the reaction solution was added dropwise to a mixture of 1.8 liters of methanol and 0.6 liters of water, and after stirring for 15 minutes, the polyimide resin was filtered. Next, the resin was reslurried in 1 liter of water and filtered, and then reslurried again in 1 liter of methanol, filtered, and dried under reduced pressure at 40°C for 8 hours. Subsequently, the dried resin was dissolved in 250 g of tetrahydrofuran, and 40 g of ion exchange resin (MB-1: manufactured by Organo Corporation) was added. The mixture was stirred for 4 hours, and the ion exchange resin was removed by filtration. The polyimide resin was precipitated in 2 liters of methanol and stirred for 15 minutes. The polyimide resin was collected by filtration and dried under reduced pressure at 45°C for 1 day to obtain polyimide (AC-1). Polyimide (AC-1) is a resin having a repeating unit represented by the following formula (AC-1). The structure of the repeating unit is 1 The weight average molecular weight of the resulting polyimide (AC-1) was 19,500, the number average molecular weight was 7,450, the phenolic hydroxyl value was 0.370 mmol / g, and ΔIm was 3.1%.
[0297] Examples and Comparative Examples In each example, the components listed in the table were mixed to obtain a resin composition. In each comparative example, the components listed in the table were mixed to obtain a comparative composition. Specifically, the content of each component listed in the table other than the solvent was the amount (parts by mass) listed in the "Parts by Mass" column of each column in the table. The content of the solvent was the amount such that the solids concentration of the composition was the "Solids Concentration (% by mass)" in the table. The ratio of the amount of each solvent used was the content ratio (mass ratio) listed in the "Ratio" column in the table. The obtained resin composition and comparative composition were pressure-filtered using a polytetrafluoroethylene filter with a pore width of 0.8 μm. In the table, "-" indicates that the composition did not contain the corresponding component.
[0298]
[0299]
[0300]
[0301]
[0302] Details of each component listed in the table are as follows:
[0303] [Resins] A-1 to A-20, AC-1: Polyimides A-1 to A-20, AC-1 synthesized above A-1 to A-20 are compounds that fall under the category of specific resins.
[0304] [Polymerizable compounds] B-1: SR-209 (manufactured by Sartomer Corporation) B-2: ADPH: dipentaerythritol hexaacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.) B-3: Compound having the following structure B-4: Compound having the following structure
[0305] [Polymerization initiators] C-1: IRGACURE OXE 01 (manufactured by BASF) C-2: IRGACURE OXE 02 (manufactured by BASF) C-3: IRGACURE 369 (manufactured by BASF) C-4: Compound having the following structure C-5: Compound having the following structure C-6: Compound having the following structure C-7: Omnirad 1312 (manufactured by IGM) C-8: Omnirad TPO H (manufactured by IGM) C-9: CPI-310FG (manufactured by San-Apro Ltd.) C-10: CPI-310B (manufactured by San-Apro Ltd.) C-11: Benzoyl peroxide (manufactured by Tokyo Chemical Industry Co., Ltd.)
[0306] [Thermal Base Generators] D-1 to D-7: Compounds represented by the following formulas (D-1) to (D-7):
[0307] [Polymerization inhibitors] E-1: 2-nitroso-1-naphthol (manufactured by Tokyo Chemical Industry Co., Ltd.) E-2: parabenzoquinone (manufactured by Tokyo Chemical Industry Co., Ltd.) E-3: paramethoxyphenol (manufactured by Tokyo Chemical Industry Co., Ltd.) E-4: compound having the following structure E-5: compound having the following structure
[0308] [Migration inhibitors] F-1 to F-8: Compounds having the following structures.
[0309] [Silane coupling agents] G-1 to G-4: Compounds having the following structures. In the following structural formulas, Et represents an ethyl group. G-5: X-12-1293 (manufactured by Shin-Etsu Chemical Co., Ltd.) G-6: KR-513 (manufactured by Shin-Etsu Chemical Co., Ltd.)
[0310] [Solvents] GBL: γ-butyrolactone DMSO: dimethyl sulfoxide NMP: N-methyl-2-pyrrolidone EL: ethyl lactate GVL: γ-valerolactone MDMPA: KJCMPA-100 (manufactured by KJ Chemicals Co., Ltd.) CP: cyclopentanone CH: cyclohexanone
[0311] [Additives] H-1: Compound having the following structure H-2: N-phenyldiethanolamine H-3: Compound having the following structure H-4: Compound having the following structure H-5: Compound having the following structure
[0312] H-5 was synthesized based on the following synthesis method. [Synthesis method of H-5] 29.72 g (70 mmol) of 4,4'-(1-(2-(4-hydroxyphenyl)-2-propyl)phenyl)ethylidene)bisphenol (Tris-PA, manufactured by Honshu Chemical Industry Co., Ltd.) was added to a flask. Next, 46.93 g (174.9 mmol) of 1,2-naphthoquinone diazide-5-sulfonic acid chloride and 17.9 g of triethylamine were dissolved in 300 g of acetone with stirring, and the solution was added dropwise to the flask using a dropping funnel over 30 minutes, followed by stirring for 30 minutes at an internal temperature of 30°C. Next, hydrochloric acid was added dropwise, and the mixture was stirred for an additional 30 minutes. Next, a solution of 1,640 g of pure water and 30 g of hydrochloric acid was prepared in a beaker, and the filtrate obtained by filtering the hydrochloride salt from the reaction solution was added dropwise to the solution. The precipitate was filtered, washed with water, and vacuum-dried at 40°C for 50 hours to obtain diazonaphthoquinone compound H-5.
[0313] [Titanium compounds] I-1: TC-750 (manufactured by Matsumoto Fine Chemical Co., Ltd.) I-2: TC-401 (manufactured by Matsumoto Fine Chemical Co., Ltd.) I-3: TC-800 (manufactured by Matsumoto Fine Chemical Co., Ltd.) I-4: TC-810 (manufactured by Matsumoto Fine Chemical Co., Ltd.) I-5 to I-8: Compounds having the following structures
[0314] <Evaluation> [Evaluation of dielectric loss tangent (Df)] Each resin composition or each comparative composition prepared in each Example and Comparative Example was applied to a 12-inch silicon wafer by spin coating to form a resin composition layer. The silicon wafer to which the obtained resin composition layer was applied was dried on a hot plate at 100°C for 5 minutes to form a resin composition layer of a uniform thickness shown in the "Film thickness (μm)" column in the table on the silicon wafer. The resin composition layer on the silicon wafer was applied with a stepper (Nikon NSR 2005 i9C) at 500 mJ / cm 2The entire surface was exposed to light with an exposure energy of 1000 kJ / min. The exposed resin composition layer (resin layer) was heated in a nitrogen atmosphere at a temperature increase rate of 10°C / min and heated at the temperature shown in the "Cure Temperature (°C)" column for the "Cure Time (min)" column in the table to obtain a cured layer (resin layer) of the resin composition layer. The cured cured layer (resin film) was immersed in a 4.9% by mass aqueous solution of hydrofluoric acid, and the cured film was peeled off from the silicon wafer. The relative permittivity (Dk) and dielectric loss tangent (Df) of the film sample at 28 GHz were measured using a resonator perturbation method. The dielectric loss tangent (Df) was evaluated according to the following evaluation criteria, and the evaluation results are shown in the "Df" column in the table. <Measurement Method> Split Cylinder Resonator (CR-728) (Device Configuration) Network Analyzer: N5230A (Keysight Corporation) (Evaluation Criteria) Dielectric Loss Tangent (Df) A: The dielectric loss tangent (Df) was less than 0.015. B: The dielectric loss tangent (Df) was 0.015 to less than 0.02. C: The dielectric loss tangent (Df) was 0.02 or more.
[0315] [Evaluation of Metal Adhesion] Each resin composition or each comparative composition prepared in each Example and Comparative Example was applied in the form of a layer on a copper substrate by spin coating to form a resin composition layer or a comparative composition layer. The copper substrate on which the resulting resin composition layer or comparative composition layer was formed was dried on a hot plate at 100°C for 5 minutes to form a resin composition layer or comparative composition layer on the copper substrate having a thickness shown in the "Film Thickness (μm)" column in the table and having a uniform thickness. The resin composition layer or comparative composition layer on the copper substrate was then heated to 500 mJ / cm using a stepper (Nikon NSR 2005 i9C). 2The sample was exposed to i-rays using a photomask with a 100 μm square unmasked area formed at an exposure energy of 1000 μm, and then developed for 60 seconds with the developer listed in the "Developer" column of the table. The resulting solution was then rinsed with propylene glycol monomethyl ether acetate (PGMEA) to obtain a 100 μm square resin layer. Furthermore, the sample was heated in a heated oven under a nitrogen atmosphere at the temperature listed in the "Cure Temperature (°C)" column of the table for the time listed in the "Cure Time (min)" column of the table to form a resin layer (pattern). The shear force of the 100 μm square resin layer on the copper substrate was measured using a bond tester (CondorSigma, manufactured by XYZTEC) in an environment of 25°C and 65% relative humidity (RH). The greater the shear force, the better the metal adhesion (copper adhesion) of the cured film. In all examples and comparative examples, the shear force exceeded 30 gf.
[0316] [Evaluation of Adhesion Strength after HTS (High Temperature Storage Test)] The resin layer and copper substrate were heated at the temperature listed in the "Cure Temperature (°C)" column for the time listed in the "Cure Time (min)" column of the table, and then left in a thermostatic chamber at 175°C for 1,000 hours. The shear force was measured and the metal adhesion after heating was evaluated using the same evaluation method as described above for the evaluation of metal adhesion. The measured shear force was evaluated according to the following evaluation criteria, and the evaluation results are listed in the "Reliability (Adhesion Strength after HTS)" column of the table. The higher the shear force, the better the metal adhesion (copper adhesion) of the cured film. Furthermore, excellent post-HTS adhesion results indicate that peeling between the cured film and the metal is less likely to occur even after a long period of time has passed. (Evaluation Criteria) A: The shear force exceeded 30 gf. B: The shear force was greater than 25 gf but not more than 30 gf. C: The shear force was not more than 25 gf. Also, 1 gf is 0.00980665 N.
[0317] [Elongation at break] In each example and comparative example, each resin composition or each comparative composition was applied in the form of a layer on a silicon wafer by spin coating to form a resin composition layer or a comparative composition layer. The silicon wafer to which the obtained resin composition layer or comparative composition layer was applied was dried on a hot plate at 100°C for 5 minutes to form a resin composition layer or comparative composition layer having a uniform thickness on the silicon wafer as shown in the "Film thickness (μm)" column in the table. The resin composition layer or comparative composition layer on the silicon wafer was formed by spin coating at 500 mJ / cm using a stepper (Nikon NSR 2005 i9C). 2 The exposed resin composition layer or comparative composition layer was heated at an exposure energy of 10°C / min under a nitrogen atmosphere using a hot plate. After reaching the temperature listed in the "Cure Temperature (°C)" column in the table, this temperature was maintained for the time listed in the "Cure Time (min)" column in the table to obtain a cured resin layer. The cured resin layer was immersed in a 4.9% by mass hydrofluoric acid solution, and the resin layer was peeled off from the silicon wafer to obtain Resin Film 1. Resin Film 1 was punched out using a punching tool to produce a film with a sample width of 10 mm and a sample length of 50 mm. The breaking elongation of the film was measured in accordance with JIS-K6251:2017 in the longitudinal and transverse directions of the film at a crosshead speed of 300 mm / min under an environment of 25°C and 65% relative humidity (RH) using a tensile tester (Tensilon). The breaking elongation was calculated by Eb (%) = (Lb - L0) / L0 x 100 (Eb: elongation at break, L0: length of the test piece before the test, Lb: length of the test piece when it was broken). The breaking elongation in the longitudinal direction was measured 10 times, and the arithmetic mean value of the 10 breaking elongation (Eb) values was used as the index value. The evaluation was performed according to the following evaluation criteria. The larger the index value, the better the breaking elongation. The evaluation results are shown in the "breaking elongation" column in the table. - Evaluation criteria - A: The index value exceeded 60%. B: The index value was greater than 40% and was 60% or less. C: The index value was 40% or less.
[0318] Example 101 The resin composition used in Example 1 was applied in the form of a layer by spin coating to the surface of the thin copper layer of a resin substrate having a thin copper layer formed on its surface. The resulting layer was dried at 100°C for 5 minutes to form a 20 μm-thick photosensitive film, which was then exposed using a stepper (Nikon Corporation, NSR1505 i6). The exposure was performed at a wavelength of 365 nm through a mask (a binary mask with a 1:1 line-and-space pattern and a line width of 10 μm). After the exposure, the film was developed with cyclopentanone for 2 minutes and rinsed with PGMEA for 30 seconds to obtain a layer pattern. The temperature was then increased at a rate of 10°C / min in a nitrogen atmosphere until it reached 230°C, at which point it was maintained at 230°C for 180 minutes to form an interlayer insulating film for a redistribution layer. This interlayer insulating film for a redistribution layer had excellent insulating properties. Furthermore, a semiconductor device was manufactured using this interlayer insulating film for a redistribution layer, and it was confirmed to operate without any problems.
Claims
1. A resin composition comprising: a resin which contains a repeating unit represented by the following formula (1-1), which contains a group having an ethylenically unsaturated bond, and which has a phenolic hydroxyl group content of 0.250 mmol / g or less; and a polymerizable compound having an ethylenically unsaturated bond. In formula (1-1), X 1 represents a tetravalent organic group; Y 1 represents a divalent organic group.
2. The resin composition according to claim 1, wherein the resin contains a repeating unit represented by the following formula (1-2) as the repeating unit represented by the formula (1-1): In formula (1-2), X 1 represents a tetravalent organic group; Y 2 represents a group containing a group represented by the following formula (2-1). In formula (2-1), R 1 and R 2 each independently represents a group having an ethylenically unsaturated bond, L represents a single bond or a divalent linking group not containing an imido bond, and * represents a bonding site to another structure.
3. The resin composition according to claim 1, wherein the resin contains a group having a vinylphenyl group as the group having an ethylenically unsaturated bond.
4. A resin composition comprising a resin containing a repeating unit represented by the following formula (1-3) and containing a vinylphenyl group, and a polymerizable compound having an ethylenically unsaturated bond: In formula (1-3), X 1 represents a tetravalent organic group; Y 3 represents a group containing a group represented by the following formula (2-2). In formula (2-2), R 1 and R 2 each independently represents a group having an ethylenically unsaturated bond, L is a single bond, -C(CH 3 ) 2 -, or -C(CF 3 ) 2 - and * represent the binding site with other structures, respectively.
5. The resin composition according to any one of claims 1 to 4, wherein the resin has a structure represented by any one of the following formulas (3-1) to (3-3). In formula (3-1), X 31 represents a tetravalent organic group; Y 31 represents a divalent organic group; R 31 represents a group having an ethylenically unsaturated bond, and * represents a bonding site with another structure. 31 represents a tetravalent organic group; Y 31 represents a divalent organic group; R 31 represents a group having an ethylenically unsaturated bond, and * represents a bonding site with another structure. 31 represents a tetravalent organic group; Y 31 represents a divalent organic group; R 32 and R 33 each independently represents -OH or a monovalent organic group; R 32 and R 33 At least one of the groups is a group having an ethylenically unsaturated bond, and * represents a bonding site with another structure.
6. The resin composition according to any one of claims 1 to 4, wherein the resin is a resin in which the rate of change in imide value calculated by the following formula before and after heating at 350°C and 1 atmospheric pressure for 1 hour is 25% or less: Rate of change (%) = (Im2 - Im1) x 100 / Im1 Im1: imide value (mmol / g) before heating Im2: imide value (mmol / g) after heating at 350°C and 1 atmospheric pressure for 1 hour 7. The above X 1 is an organic group containing a structure in which two or more hydrogen atoms have been removed from a structure represented by any one of formulas (V-1) to (V-4). The resin composition according to any one of claims 1 to 4. In formula (V-2), R X1 Each of R independently represents a hydrogen atom, an alkyl group, or a halogenated alkyl group. X2 and R X3 each independently represents a hydrogen atom or a substituent; R X2 and R X3 may be linked to form a ring structure.
8. The resin composition according to any one of claims 1 to 4, which contains an azole compound.
9. A diamine compound represented by the following formula (4-1): In formula (4-1), R 3 and R 4 each independently represents a group having an ethylenically unsaturated bond; R 3 and R 4 At least one of the groups has an aromatic hydrocarbon group, and L is a single bond, -C(CH 3 ) 2 - or - C(CF 3 ) 2 Represents -.
10. The above R 3 and R 4 The diamine compound according to claim 9 , wherein each independently has a vinylphenyl group.
11. A resin composition comprising a resin which is a reaction product of the diamine compound according to claim 9 with a compound having a total of two or more carboxy groups and carboxylic anhydride groups or a derivative thereof, and a polymerizable compound having an ethylenically unsaturated bond.
12. The resin composition according to any one of claims 1 to 4 and 11, which is used for forming an interlayer insulating film for a rewiring layer.
13. A cured product obtained by curing the resin composition according to any one of claims 1 to 4 and 11.
14. A laminate comprising two or more layers of the cured product according to claim 13, and including a metal layer between any two of the layers of the cured product.
15. A method for producing a cured product, comprising a film-forming step of applying the resin composition according to any one of claims 1 to 4 and 11 onto a substrate to form a film.
16. The method for producing a cured product according to claim 15, comprising an exposure step of selectively exposing the film to light, and a development step of developing the film with a developer to form a pattern.
17. A method for producing a cured product according to claim 15, comprising a heating step of heating the film at 50 to 450°C.
18. A method for producing a laminate, comprising the method for producing the cured product according to claim 15.
19. A method for producing a semiconductor device, comprising the method for producing the cured product according to claim 15.
20. A semiconductor device comprising the cured product according to claim 13.
Citation Information
Patent Citations
Modified maleimide compound, and prepreg and laminated board prepared from modified maleimide compound
CN112079763A
Hybrid polymer material for liquid crystal alignment layer
JP2006512422A
Polyimide, resin composition, resin film, laminate, coverlay film, copper foil with resin, metal-clad laminate, and circuit board
JP2022150088A
Photosensitive resin composition and cured film
WO2010110335A1
Photosensitive resin composition and method for producing cured relief pattern
WO2018037997A1