Hot-melt adhesive composition and adhesive tape

The hot melt adhesive composition, featuring a partially hydrogenated styrene-butadiene block copolymer and tailored tackifiers, addresses the heat resistance and adhesion issues of conventional adhesives, providing stable adhesion and low viscosity in high-temperature environments for efficient hot-melt coating.

WO2024203719A1PCT designated stage expired Publication Date: 2024-10-03DENKA CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011013
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-21
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional rubber-based hot melt adhesives exhibit poor heat resistance and adhesive deterioration in high-temperature environments, and acrylic adhesives struggle with adhesion to olefin resin materials like polyethylene and polypropylene, leading to instability in hot-melt coating processes.

Method used

A hot melt adhesive composition incorporating a partially hydrogenated styrene-butadiene block copolymer and a combination of tackifiers, including terpene resins and rosin esters, with specific molecular weight ranges and softening points, along with an antioxidant, to maintain low viscosity and high adhesion in high-temperature environments.

Benefits of technology

The adhesive composition demonstrates stable adhesion to olefin resin materials and maintains low viscosity during long-term heating, ensuring effective hot-melt coating and high adhesive strength at elevated temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

The present invention provides a hot-melt adhesive composition which has little viscosity increase associated with long-time heating and is suitable for use in hot-melt coating, while exhibiting high adhesion to an olefin resin material in a high temperature environment. According to the present invention, provided is a hot-melt adhesive composition which contains a styrene-butadiene block copolymer and a tackifier, wherein: the styrene-butadiene block copolymer is partially hydrogenated in the butadiene moiety; and the chemiluminescence intensity at 5 minutes after the start of measurement in an atmosphere at 185°C is less than 300,000 count / s.
Need to check novelty before this filing date? Find Prior Art

Description

Hot melt adhesive composition and adhesive tape

[0001] The present invention relates to a hot melt pressure sensitive adhesive composition and a pressure sensitive adhesive tape.

[0002] In various industrial fields such as electrical appliances, automobiles, and construction, adhesive tapes are used for purposes such as joining various assembly components. The adhesives used in double-sided adhesive tapes include acrylic adhesives and rubber adhesives, with acrylic adhesives being the most widely used. However, acrylic adhesives have a problem in that they have low adhesive strength to olefin resin materials such as polyethylene and polypropylene, the use of which has been increasing in recent years.

[0003] Rubber-based pressure-sensitive adhesives exhibit high adhesive strength to olefin-based resin materials that are difficult to adhere to with acrylic-based pressure-sensitive adhesives. Patent Document 1 discloses a pressure-sensitive adhesive composition having a base polymer that is a block copolymer of a monovinyl-substituted aromatic compound and a conjugated diene compound.

[0004] JP 2013-216853 A

[0005] Conventional rubber-based pressure-sensitive adhesives have the problem of insufficient heat resistance and a tendency for their adhesive properties to deteriorate in high-temperature environments. In addition, when the pressure-sensitive adhesive composition is hot-melt coated in the production of pressure-sensitive adhesive tapes, the viscosity of the pressure-sensitive adhesive composition increases due to prolonged heating, making stable coating difficult.

[0006] The present invention has been made in view of the above circumstances, and aims to provide a hot-melt pressure-sensitive adhesive composition that exhibits little increase in viscosity upon prolonged heating, can be suitably used for hot-melt coating, and exhibits high adhesive strength to olefin-based resin materials in high-temperature environments.

[0007] [1] A hot-melt pressure-sensitive adhesive composition comprising a styrene-butadiene block copolymer and a tackifier, wherein the styrene-butadiene block copolymer has a partially hydrogenated butadiene moiety, and wherein the chemiluminescence intensity at 5 minutes after the start of measurement in an atmosphere at 185°C is less than 300,000 counts / s. [2] The hot-melt pressure-sensitive adhesive composition according to [1], which has a viscosity at 185°C of 10,000 to 100,000 mPa·s. [3] The hot-melt pressure-sensitive adhesive composition according to [1] or [2], which contains an antioxidant. [4] The hot-melt pressure-sensitive adhesive composition according to [3], wherein the antioxidant has a melting point of 60°C or higher. [5] The hot melt pressure-sensitive adhesive composition according to any one of [1] to [4], wherein the tackifier comprises a first tackifier, the first tackifier being at least one of a terpene resin that is liquid at 23° C. and a rosin ester that is liquid at 23° C. [6] The hot melt pressure-sensitive adhesive composition according to any one of [1] to [5], wherein the tackifier comprises a second tackifier, the second tackifier having a softening point of 70 to 120° C. [7] The hot melt pressure-sensitive adhesive composition according to any one of [1] to [6], wherein the tackifier comprises a third tackifier, the third tackifier having a softening point of 140° C. or higher. [8] The hot melt pressure-sensitive adhesive composition according to any one of [1] to [4], wherein the tackifier comprises a first tackifier, a second tackifier, and a third tackifier, wherein the first tackifier is a terpene resin that is liquid at 23° C., the second tackifier is a terpene resin having a softening point of 70 to 120° C., and the third tackifier is a terpene phenol resin having a softening point of 140° C. or higher. [9] The hot melt pressure-sensitive adhesive composition according to [8], wherein the hot melt pressure-sensitive adhesive composition contains 45 to 55 parts by mass of the styrene-butadiene block copolymer, 10 to 20 parts by mass of the first tackifier, 10 to 25 parts by mass of the second tackifier, and 17.5 to 27.5 parts by mass of the third tackifier, relative to 100 parts by mass of the hot melt pressure-sensitive adhesive composition.

[10] The hot-melt pressure-sensitive adhesive composition according to [8] or [9], wherein the content ratio of the first tackifier to the second tackifier in the hot-melt pressure-sensitive adhesive composition is 1:0.5 to 1:1.5 by mass.

[11] The hot-melt pressure-sensitive adhesive composition according to any one of [1] to

[10] , wherein the styrene-butadiene block copolymer has a content of styrene-derived monomer units of 24 mass% or more.

[12] The hot-melt pressure-sensitive adhesive composition according to any one of [1] to

[11] , wherein the styrene-butadiene block copolymer contains: a component a having a peak top molecular weight of 200,000 or more and 400,000 or less, and a component b having a peak top molecular weight of 100,000 or more and less than 200,000, as measured by GPC.

[13] A pressure-sensitive adhesive tape comprising a pressure-sensitive adhesive layer comprising the hot-melt pressure-sensitive adhesive composition according to any one of [1] to

[12] .

[0008] As a result of extensive research, the present inventors have found that a hot melt pressure sensitive adhesive composition containing a styrene-butadiene block copolymer in which the butadiene moiety is partially hydrogenated and a tackifier, and having a chemiluminescence emission intensity that satisfies specific conditions, exhibits a small increase in viscosity with prolonged heating and has good adhesive strength to olefin resin materials in high temperature environments, leading to the completion of the present invention.

[0009] The following describes embodiments of the present invention. The features of the embodiments described below can be combined with each other. Each feature can also be an invention independently.

[0010] 1. Hot-melt pressure-sensitive adhesive composition The hot-melt pressure-sensitive adhesive composition according to the present invention (hereinafter simply referred to as the pressure-sensitive adhesive composition) contains a styrene-butadiene block copolymer and a tackifier. In the present invention, the term "tackifier" refers to a tackifier, which is a thermoplastic resin that is liquid or solid at room temperature and is added to enhance adhesiveness.

[0011] 1.1. Styrene-Butadiene Block Copolymer The styrene-butadiene block copolymer contained in the PSA composition has a partially hydrogenated butadiene moiety. The styrene-butadiene block copolymer according to the present invention refers to a block copolymer including a block having a styrene monomer unit and a block having a butadiene monomer unit. The styrene monomer unit is a structural unit (monomer unit) of the block and copolymer derived from styrene. The butadiene monomer unit is a structural unit (monomer unit) of the block and copolymer derived from butadiene.

[0012] The styrene-butadiene block copolymer preferably has a styrene monomer unit content of 24% by mass or more, more preferably 24 to 40% by mass, based on 100% by mass of the styrene-butadiene block copolymer. Specific examples of the styrene monomer unit content include 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, and 40% by mass, and may be within a range between any two of the values ​​exemplified here. Furthermore, the styrene-butadiene block copolymer preferably has a butadiene monomer unit content of 76% by mass or less, more preferably 50 to 76% by mass, based on 100% by mass of the styrene-butadiene block copolymer. The styrene monomer unit content is, for example, 50, 55, 56, 57, 58, 59, 60, 61, 62, 63, 64, 65, 66, 67, 68, 69, 70, 71, 72, 73, 74, 75, or 76% by mass, and may be within a range between any two of the values ​​exemplified here. By setting the styrene monomer unit or butadiene monomer unit content within the above numerical range, the resulting pressure-sensitive adhesive tape will have appropriate adhesive strength and holding power to the adherend. The styrene monomer unit and butadiene monomer unit contents can be measured in accordance with JIS K6383.

[0013] The butadiene portion of the styrene-butadiene block copolymer is preferably hydrogenated by 20 to 90 mass%, more preferably by 30 to 80 mass%. A specific example of the styrene-butadiene block copolymer in which the butadiene portion is partially hydrogenated is a styrene-butadiene-butylene-styrene block copolymer (SBBS).

[0014] The PSA composition preferably contains, as the styrene-butadiene block copolymer, a triblock copolymer including block A containing monomer units derived from styrene, block B containing monomer units derived from butadiene, and block C containing monomer units derived from styrene. Furthermore, the PSA composition according to the present invention preferably contains, as the styrene-butadiene block copolymer, a diblock copolymer including block A containing monomer units derived from styrene and block B containing monomer units derived from butadiene. Here, the block B containing monomer units derived from butadiene is preferably partially hydrogenated. That is, the block B containing monomer units derived from butadiene preferably has a butadiene block and a butylene block.

[0015] The pressure-sensitive adhesive composition according to the present invention preferably contains 50 to 85 mass% of the diblock copolymer, and more preferably 55 to 80 mass%, when the total mass of the styrene-butadiene block copolymers contained in the pressure-sensitive adhesive composition is taken as 100 mass%. Specific examples of the diblock copolymer content include 50, 55, 60, 65, 70, 75, 80, and 85 mass%, and may be within a range between any two of the values ​​exemplified here. By ensuring that the diblock copolymer content falls within the above range, a pressure-sensitive adhesive composition with appropriate tack can be obtained.

[0016] The styrene-butadiene block copolymer preferably contains a component a having a peak top molecular weight of 200,000 or more and 400,000 or less in GPC measurement (gel permeation chromatography), and a component b having a peak top molecular weight of 100,000 or more and less than 200,000. In GPC measurement, containing component a and component b means that the GPC spectrum obtained by GPC measurement has a peak whose top is at a molecular weight of 200,000 or more and 400,000 or less, and a peak whose top is at a molecular weight of 100,000 or more and less than 200,000.

[0017] Component a is, for example, a component having a peak top molecular weight of 200,000, 210,000, 220,000, 230,000, 240,000, 250,000, 260,000, 270,000, 280,000, 290,000, 300,000, 310,000, 320,000, 330,000, 340,000, 350,000, 360,000, 370,000, 380,000, 390,000, or 400,000, and may be within a range between any two of the numerical values ​​exemplified here. Component b is, for example, a component having a peak top molecular weight of 100,000, 110,000, 120,000, 130,000, 140,000, 150,000, 160,000, 170,000, 180,000, or 190,000, or a component less than 200,000, and may be within a range between any two of the numerical values ​​exemplified here. By including component a and component b, it is possible to obtain an adhesive tape that has an excellent balance of adhesive strength to olefin-based materials and adhesive strength at high temperatures.

[0018] The styrene-butadiene block copolymer may contain components other than the components a and b in GPC measurement. As an example, the styrene-butadiene block copolymer may further contain a component having a peak top molecular weight of 5,000 or more and less than 100,000, for example, a component of 5,000, 10,000, 20,000, 30,000, 40,000, 50,000, 60,000, 70,000, 80,000, or 90,000, or a component less than 100,000, or may contain a component having a peak top molecular weight within a range between any two of the numerical values ​​exemplified here.

[0019] A styrene-butadiene block copolymer having such a molecular weight distribution can be obtained, for example, by appropriately selecting and combining two or more styrene-butadiene block copolymers having different peak top molecular weights, weight average molecular weights, or molecular weight distributions. The pressure-sensitive adhesive composition can contain two or more styrene-butadiene block copolymers as the styrene-butadiene block copolymer. For example, the pressure-sensitive adhesive composition can contain, as the styrene-butadiene block copolymer, a styrene-butadiene block copolymer A having a peak top molecular weight of 200,000 or more and 400,000 or less, and a styrene-butadiene block copolymer B having a peak top molecular weight of 100,000 or more and less than 200,000. In this case, the styrene-butadiene block copolymer A corresponds to the above-mentioned component a, and the styrene-butadiene block copolymer B corresponds to the above-mentioned component b.

[0020] The butadiene portion of the styrene-butadiene block copolymer A is partially hydrogenated, and preferably 20 to 90 mass% of the butadiene portion of the styrene-butadiene block copolymer A is hydrogenated, and more preferably 30 to 80 mass%. A specific example of a styrene-butadiene block copolymer in which the butadiene portion is partially hydrogenated is styrene-butadiene-butylene-styrene block copolymer (SBBS). The hydrogenation rate can be determined from the peak of hydrogenated butadiene and peaks derived from other monomer units in composition analysis by H-NMR.

[0021] The PSA composition preferably contains, as the styrene-butadiene block copolymer A, a triblock copolymer including a block α containing monomer units derived from styrene, a block β containing monomer units derived from butadiene, and a block γ containing monomer units derived from styrene. The PSA composition also preferably contains, as the styrene-butadiene block copolymer A, a diblock copolymer including a block β containing monomer units derived from α-butadiene, which contains monomer units derived from styrene. Here, the block β is preferably partially hydrogenated, i.e., the block β preferably has a butadiene block and a butylene block. The styrene-butadiene block copolymer A preferably contains 50 to 85 mass%, more preferably 55 to 80 mass%, of the diblock copolymer, based on 100 mass% of the styrene-butadiene block copolymer A. The content of the diblock copolymer is, for example, 50, 55, 60, 65, 70, 75, 80, or 85 mass%, and may be within a range between any two of the values ​​exemplified herein.

[0022] The styrene-butadiene block copolymer A has a peak top molecular weight of 200,000 or more and 400,000 or less in GPC measurement, and specifically, for example, the peak top molecular weight is 200,000, 210,000, 220,000, 230,000, 240,000, 250,000, 260,000, 270,000, 280,000, 290,000, 300,000, 310,000, 320,000, 330,000, 340,000, 350,000, 360,000, 370,000, 380,000, 390,000, or 400,000, and may be within a range between any two of the numerical values ​​exemplified here.

[0023] The styrene-butadiene block copolymer A preferably has an MFR (melt flow rate) measured at 200°C and 5 kgf of less than 10 g / 10 min. The styrene-butadiene block copolymer A may have an MFR measured at 200°C and 5 kgf of, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9 g / 10 min, or less than 10 g / 10 min, or may be within a range between any two of the values ​​exemplified here.

[0024] The styrene-butadiene block copolymer B has a partially hydrogenated butadiene portion, preferably 20 to 90 mass % hydrogenated, more preferably 30 to 80 mass % hydrogenated. A specific example of the styrene-butadiene block copolymer having a partially hydrogenated butadiene portion is a styrene-butadiene-butylene-styrene block copolymer (SBBS).

[0025] The PSA composition preferably contains, as the styrene-butadiene block copolymer B, a triblock copolymer including a block α containing monomer units derived from styrene, a block β containing monomer units derived from butadiene, and a block γ containing monomer units derived from styrene. The PSA composition also preferably contains, as the styrene-butadiene block copolymer B, a diblock copolymer including a block β containing monomer units derived from styrene and a block α containing monomer units derived from butadiene. Here, the block β is preferably partially hydrogenated; that is, the block β containing monomer units derived from butadiene preferably has a butadiene block and a butylene block. The styrene-butadiene block copolymer B preferably contains 50 to 85 mass %, more preferably 55 to 80 mass %, of the diblock copolymer, when the styrene-butadiene block copolymer B is taken as 100 mass %. The content of the diblock copolymer is specifically, for example, 50, 55, 60, 65, 70, 75, 80, or 85% by mass, and may be within a range between any two of the values ​​exemplified here.

[0026] The styrene-butadiene block copolymer B has a peak top molecular weight of 100,000 or more and less than 200,000 as measured by GPC. Specifically, for example, the peak top molecular weight is a component of 100,000, 110,000, 120,000, 130,000, 140,000, 150,000, 160,000, 170,000, 180,000, or 190,000, or a component of less than 200,000, and may be within a range between any two of the numerical values ​​exemplified here.

[0027] The styrene-butadiene block copolymer B preferably has an MFR of 10 g / 10 min or more measured at 200° C. and 5 kgf. The styrene-butadiene block copolymer B may have an MFR of, for example, 10, 12, 13, 14, 15, 16, 17, 18, 19, or 20 g / 10 min measured at 200° C. and 5 kgf, and may be within a range between any two of the values ​​exemplified here.

[0028] The styrene-butadiene block copolymer may be used alone or in combination of two or more. For example, two or more styrene-butadiene block copolymers having different peak top molecular weights, weight average molecular weights, molecular weight distributions, MFRs, contents of styrene-derived monomer units, contents of diblock copolymers, etc. may be used in combination.

[0029] 1.2. First Tackifier The PSA composition preferably contains a first tackifier. The first tackifier is at least one of a terpene resin that is liquid at 23°C and a rosin ester that is liquid at 23°C. It is more preferable to use a terpene resin that is liquid at 23°C as the first tackifier. The PSA composition may contain one type of first tackifier alone, or two or more types in combination.

[0030] The terpene resin according to the present invention refers to a terpene polymer, a copolymer of terpene and other monomers, and hydrogenated versions of these polymers, and examples thereof include terpene resins, aromatic modified terpene resins, terpene phenolic resins, and hydrogenated terpene phenolic resins. Examples of terpene resins that are liquid at 23°C include YS Resin LP (aromatic modified terpene resin, flash point 220°C, manufactured by Yasuhara Chemical Co., Ltd.), Dimalon (liquid terpene resin, flash point 174°C, manufactured by Yasuhara Chemical Co., Ltd.), YS Resin CP (liquid terpene resin, flash point 178°C, manufactured by Yasuhara Chemical Co., Ltd.), YS Resin PX300N (terpene resin, flash point 202°C, manufactured by Yasuhara Chemical Co., Ltd.), and YS Polystar T30 (terpene phenolic resin, flash point 205°C, manufactured by Yasuhara Chemical Co., Ltd.). Among these, YS Resin LP is preferred from the viewpoints of its high flash point, low heat loss, and high compatibility with styrene-butadiene block copolymers. The flash point of the terpene resin that is liquid at 23°C is preferably 180°C or higher, more preferably 200°C or higher, and even more preferably 210°C or higher.

[0031] Examples of rosin esters that are liquid at 23° C. include Super Ester A-18 (manufactured by Arakawa Chemical Industries, Ltd.) and Ester Gum AT (manufactured by Arakawa Chemical Industries, Ltd.).

[0032] The viscosity of the first tackifier at 25° C. is preferably 500 to 150,000 mPa·s, and more preferably 1,000 to 100,000 mPa·s. The viscosity at 25° C. may be, for example, 500, 1,000, 2,000, 5,000, 10,000, 20,000, 50,000, 100,000, 120,000, or 150,000 mPa·s, or may be within a range between any two of the values ​​exemplified here.

[0033] 1.3. Second Tackifier The pressure-sensitive adhesive composition preferably contains a second tackifier. The second tackifier has a softening point of 70 to 120°C. The pressure-sensitive adhesive composition may contain one type of second tackifier alone or two or more types in combination.

[0034] The softening point of the second tackifier is 70 to 120° C., preferably 80 to 120° C., and more preferably 90 to 115° C. Specific examples of the softening point include 70, 75, 80, 85, 90, 95, 100, 105, 110, 115, and 120° C., and may be within a range between any two of the values ​​exemplified here.

[0035] The second tackifier may be, for example, a C9 petroleum resin, a hydrogenated C9 petroleum resin, a C5 petroleum resin, an alicyclic petroleum resin, an alicyclic / aromatic petroleum resin, a rosin-based resin (polymerized rosin ester, modified polymerized rosin ester, stabilized rosin ester, etc.), a terpene-based resin, etc. As the second tackifier, it is preferable to use a terpene-based resin because of its good adhesiveness, and it is more preferable to use a terpene resin.

[0036] 1.4. Third Tackifier The pressure-sensitive adhesive composition preferably contains a third tackifier. The third tackifier has a softening point of 140°C or higher. The pressure-sensitive adhesive composition may contain one type of third tackifier alone or two or more types of third tackifiers in combination.

[0037] The softening point of the third tackifier is 140° C. or higher, preferably 140 to 180° C., and more preferably 160 to 170° C. Specific examples of the softening point include 140, 145, 150, 155, 160, 165, 170, 175, and 180° C., and may be within a range between any two of the values ​​exemplified here.

[0038] As the third tackifier, for example, C9 petroleum resin, hydrogenated C9 petroleum resin, C5 petroleum resin, alicyclic petroleum resin, alicyclic / aromatic petroleum resin, terpene resin, rosin resin (polymerized rosin ester, modified polymerized rosin ester, stabilized rosin ester, etc.), alkylphenol compound, etc., each having a softening point of 140°C or higher can be used. From the viewpoint of an excellent balance between melt viscosity and high-temperature adhesive strength, it is preferable to use a terpene phenol resin as the third tackifier. In particular, from the viewpoint of obtaining a pressure-sensitive adhesive composition having a low melt viscosity and being easy to apply, it is more preferable to use a terpene phenol resin having a softening point of 140°C or higher as the third tackifier.

[0039] The softening point of the tackifier can be defined as a value measured based on the softening point test method (ring and ball method) specified in JIS K5902 and JIS K2207. Specifically, the sample is melted as quickly as possible at the lowest possible temperature and carefully filled into a ring placed on a flat metal plate, avoiding the formation of bubbles. After cooling, any raised portion of the ring, including the top edge, is cut off with a slightly heated knife. Next, a holder (ring stand) is placed in a glass container (heating bath) with a diameter of at least 85 mm and a height of at least 127 mm, and glycerin is poured in to a depth of at least 90 mm. Next, a steel ball (diameter 9.5 mm, weight 3.5 g) and the ring filled with the sample are immersed in the glycerin without touching each other, and the glycerin temperature is maintained at 20°C ± 5°C for 15 minutes. Next, the steel ball is placed in the center of the surface of the sample in the ring and placed in its fixed position on the holder. Next, maintain a distance of 50 mm from the top of the ring to the glycerin surface, place a thermometer, and heat the container with the center of the thermometer's mercury bulb at the same height as the center of the ring. The flame of the Bunsen burner used for heating should be aimed midway between the center of the bottom and the edge of the container, ensuring uniform heating. The rate of increase in bath temperature after reaching 40°C from the start of heating can be set to 5.0±0.5°C per minute. The sample gradually softens, flows down from the ring, and the temperature is read when it touches the bottom plate, which can be used as the softening point. Two or more softening point measurements can be made simultaneously, and the average value can be used.

[0040] Furthermore, since the softening point is about 50°C higher than the glass transition point of the tackifier, the softening point can be estimated by detecting Tg using a DSC (differential scanning calorimeter). One method for identifying the softening point of a tackifier in an adhesive using this technique involves isolating the tackifier component in the adhesive using preparative HPLC, measuring Tg from the DSC measurement results of this isolated sample, and estimating the softening point.

[0041] 1.5. Content of Each Component The contents of the styrene-butadiene block copolymer, the first tackifier, the second tackifier, and the third tackifier in the pressure-sensitive adhesive composition are not particularly limited. As an example, by setting the contents of each component within the following ranges, a pressure-sensitive adhesive tape with even higher adhesive strength to olefin-based materials, particularly high adhesive strength at high temperatures, is likely to be obtained.

[0042] The PSA composition preferably contains 45 to 55 parts by mass of a styrene-butadiene block copolymer relative to 100 parts by mass of the PSA composition. Specific examples of the content of the styrene-butadiene block copolymer include 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, and 55 parts by mass, and may be within a range between any two of the values ​​exemplified here.

[0043] The PSA composition preferably contains 10 to 20 parts by mass of the first tackifier, based on 100 parts by mass of the PSA composition. Specific examples of the content of the first tackifier include 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, and 20 parts by mass, and may be within a range between any two of the values ​​exemplified here.

[0044] The PSA composition preferably contains 10 parts by mass or more of the second tackifier, more preferably 10 to 40 parts by mass, and even more preferably 10 to 25 parts by mass, based on 100 parts by mass of the PSA composition. Specific examples of the content of the second tackifier include 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, and 40 parts by mass, and may be within a range between any two of the numerical values ​​exemplified here.

[0045] The PSA composition preferably contains 10 to 30 parts by mass, and more preferably 17.5 to 27.5 parts by mass, of the third tackifier, based on 100 parts by mass of the PSA composition. Specific examples of the content of the third tackifier include 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, and 30 parts by mass, and may be within a range between any two of the values ​​exemplified here.

[0046] The pressure-sensitive adhesive composition preferably contains a first tackifier, a second tackifier, and a third tackifier as tackifiers, the first tackifier being a terpene resin that is liquid at 23°C, the second tackifier being a terpene resin having a softening point of 70 to 120°C, and the third tackifier being a terpene phenol resin having a softening point of 140°C or higher.

[0047] The pressure-sensitive adhesive composition preferably contains, when the pressure-sensitive adhesive composition is taken as 100 parts by mass, 45 to 55 parts by mass of a styrene-butadiene block copolymer, 10 to 20 parts by mass of a first tackifier, 10 to 25 parts by mass of a second tackifier, and 17.5 to 27.5 parts by mass of a third tackifier.

[0048] When the pressure-sensitive adhesive composition contains a first tackifier and a second tackifier, the content ratio of the first tackifier to the second tackifier is preferably 1:0.5 to 1:1.5 by mass.

[0049] 1.6. Other Components In addition to the above-described components, the pressure-sensitive adhesive composition according to the present invention may contain various additives such as plasticizers, antioxidants, UV absorbers, stabilizers, fillers, and modifiers, to the extent that the effects of the present invention are not impaired.

[0050] (Plasticizer) The PSA composition may contain a plasticizer. Examples of the plasticizer include phthalate ester-based plasticizers, polybutene, paraffin-based process oil, naphthene-based process oil, aromatic process oil, liquid paraffin, and hydrocarbon-based synthetic oil.

[0051] (Antioxidant) The pressure-sensitive adhesive composition preferably contains an antioxidant. By containing an antioxidant, it becomes easier to control the chemiluminescence emission intensity of the pressure-sensitive adhesive composition, which will be described later, to a suitable value. Examples of antioxidants include 2,6-di-t-butyl-4-methylphenol, n-octadecyl-3-(4'-hydroxy-3',5'-di-t-butylphenyl)propionate, 2,2'-methylenebis(4-methyl-6-t-butylphenol), 2,2'-methylenebis(4-ethyl-6-t-butylphenol), 2,4-bis(octylthiomethyl)-o-cresol, 2-t-butyl-6-(3-t-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate, 2,4-di-t-amyl-6-[1-(3,5-di-t-amyl-2-hydroxyphenyl)ethyl]phenyl acrylate, 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl Examples of antioxidants include phenolic antioxidants such as tetrakis[methylene-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane, 2,4-bis[(dodecylthio)methyl]-6-methylphenol, and pentaerythritol tetrakis[3-[3,5-di(tert-butyl)-4-hydroxyphenyl]propionate]; sulfur-based antioxidants such as dilauryl thiodipropionate, lauryl stearyl thiodipropionate, and pentaerythritol tetrakis(3-laurylthiopropionate); phosphorus-based antioxidants such as tris(nonylphenyl)phosphite and tris(2,4-di-t-butylphenyl)phosphite; and lactone-based antioxidants.

[0052] The antioxidant preferably has a melting point of 60° C. or higher, more preferably 80° C. or higher. The upper limit of the melting point of the antioxidant is not particularly limited, but is, for example, 300° C. or lower. When the melting point of the antioxidant is within the above range, the antioxidant is less likely to liquefy in a high-temperature environment, and this makes it possible to suppress a decrease in the adhesive strength of the pressure-sensitive adhesive composition in a high-temperature environment.

[0053] (UV Absorber) Examples of UV absorbers include benzotriazole UV absorbers such as 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-t-butylphenyl)benzotriazole, and 2-(2'-hydroxy-3',5'-di-t-butylphenyl)-5-chlorobenzotriazole, benzophenone UV absorbers such as 2-hydroxy-4-methoxybenzophenone, salicylic acid ester UV absorbers, cyanoacrylate UV absorbers, and hindered amine light stabilizers. These can be used alone or in combination.

[0054] The content of the antioxidant relative to 100 parts by mass of the PSA composition is, for example, 0.05 to 5 parts by mass, preferably 0.1 to 3.5 parts by mass, and more preferably 0.1 to 0.5 parts by mass. Specific examples of the content of the antioxidant include 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, and 5 parts by mass, and may be within a range between any two of the values ​​exemplified here.

[0055] (Filler) Examples of the filler include calcium carbonate, kaolin, talc, titanium oxide, mica, styrene beads, silica, etc. These particulate fillers can be used alone or in combination.

[0056] 1.7 Chemiluminescence Emission Intensity The pressure-sensitive adhesive composition according to the present invention has a chemiluminescence emission intensity of less than 300,000 counts / s 5 minutes after the start of measurement in an atmosphere at 185°C. Pressure-sensitive adhesive compositions having a chemiluminescence emission intensity within this range exhibit a small increase in viscosity with prolonged heating and good adhesive strength to olefin-based resin materials in high-temperature environments. The chemiluminescence emission intensity of the pressure-sensitive adhesive composition can be controlled by appropriately selecting the types of components of the pressure-sensitive adhesive composition and adjusting the amounts thereof.

[0057] Chemiluminescence is weak light that is generated when molecules in a chemical reaction system return from an excited state to a ground state, emitting the difference in energy as photons. Chemiluminescence emission intensity is measured by detecting this light. An example of a specific method for measuring chemiluminescence emission intensity 5 minutes after the start of measurement in an atmosphere at 185°C is shown below. The pressure-sensitive adhesive composition is placed in the sample chamber of a chemiluminescence measuring device (CLA-FS4, manufactured by Tohoku Electronics Industries Co., Ltd.) having a photomultiplier tube as a detection element that has been preheated to 185°C, and measurement of the chemiluminescence emission intensity is started while air with an oxygen concentration of 20% is fed into the sample chamber at a rate of 50 ml / min. The chemiluminescence emission intensity (unit: count / s) is measured 5 minutes after the start of measurement. The chemiluminescence intensity of the adhesive composition may be measured by placing an adhesive tape having an adhesive layer made of the adhesive composition in the sample chamber of a chemiluminescence measuring device with the adhesive layer (adhesive surface) facing upward.

[0058] The chemiluminescence intensity 5 minutes after the start of measurement in an atmosphere of 185 ° C. is preferably less than 200,000 counts / s, more preferably less than 150,000 counts / s. The lower limit of the chemiluminescence intensity is not particularly limited, but is, for example, 1,000 counts / s or more. The chemiluminescence intensity is, for example, 1,000, 5,000, 10,000, 20,000, 30,000, 40,000, 50,000, 100,000, 150,000, 200,000, 250,000, or less than 300,000 counts / s, and may be within a range between any two of the values ​​exemplified here.

[0059] 1.8. Viscosity The PSA composition preferably has a melt viscosity at 185°C of 10,000 to 100,000 mPa·s, more preferably 15,000 to 90,000 mPa·s. Specific examples of the melt viscosity include 10,000, 20,000, 30,000, 40,000, 50,000, 60,000, 70,000, 80,000, 90,000, and 100,000 mPa·s, and may be within a range between any two of the values ​​exemplified here. By ensuring that the melt viscosity at 185°C falls within the above range, a PSA composition suitable for hot-melt coating can be obtained.

[0060] The pressure-sensitive adhesive composition preferably has an initial viscosity η0 at 185°C of 10,000 to 100,000 mPa·s, more preferably 15,000 to 90,000 mPa·s. Here, the initial viscosity refers to the melt viscosity when the pressure-sensitive adhesive composition is heated at 185°C for a short period of time, such as 5 minutes or less. The pressure-sensitive adhesive composition preferably has a difference (η1-η0) between the melt viscosity η1 and the initial viscosity η0 when heated at 185°C for 30 minutes, such that the difference (η1-η0) is 0 to 20,000 mPa·s, more preferably 0 to 10,000 mPa·s, and even more preferably 0 to 5,000 mPa·s. In this case, the degree of viscosity increase of the pressure-sensitive adhesive composition due to prolonged heating is small, enabling stable hot-melt coating.

[0061] The melt viscosity at 185°C and the initial viscosity can be controlled by appropriately selecting the types of components of the PSA composition and adjusting the amounts of the components. The viscosity of the PSA composition can be measured using a rheometer at 185°C or room temperature and at a shear rate of 10 (1 / s).

[0062] 1.9. Manufacturing Method The manufacturing method of the PSA composition is not particularly limited. For example, the manufacturing method of the PSA composition according to this embodiment may include a tackifier kneading step in which raw materials such as a first tackifier, a second tackifier, and a third tackifier are kneaded in a kneader. In the above step, an antioxidant and a plasticizer may also be added. In the tackifier kneading step, kneading may be performed, for example, for 3 to 30 minutes at 5 to 25 rpm. The manufacturing method of the PSA composition may further include a block copolymer addition / kneading step in which a styrene-butadiene block copolymer is added and kneaded after the tackifier and other kneading step. In the block copolymer addition / kneading step, kneading may be performed, for example, for 20 to 200 minutes at 5 to 25 rpm.

[0063] 2. Pressure-sensitive Adhesive Tape The pressure-sensitive adhesive tape according to the present invention comprises a pressure-sensitive adhesive layer containing the pressure-sensitive adhesive composition.

[0064] 2.1. Structure and Manufacturing Method of Pressure-Sensitive Adhesive Tape The pressure-sensitive adhesive layer is formed by heating and melting a pressure-sensitive adhesive composition and hot-melt coating it onto a substrate. That is, the manufacturing method of a pressure-sensitive adhesive tape includes a coating step in which the pressure-sensitive adhesive composition is hot-melt coated onto a substrate to form a pressure-sensitive adhesive layer. In this case, the pressure-sensitive adhesive tape includes a pressure-sensitive adhesive layer and a substrate layer composed of the substrate. In the case of the hot-melt method, the pressure-sensitive adhesive tape can be manufactured with less energy, cost, and time than a method in which the pressure-sensitive adhesive composition is dissolved in a solvent, coated, and dried. As the coating method, a known method can be used, and a non-contact coating method or a contact coating method can be adopted. An example of a non-contact coating method is cross coating. An example of a contact coating method is slot die coating.

[0065] The thickness of the pressure-sensitive adhesive layer is not particularly limited, but is preferably 40 to 100 μm. Specific examples of the thickness of the pressure-sensitive adhesive layer include 40, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, and 100 μm, and may be within a range between any two of the values ​​exemplified here. Because the pressure-sensitive adhesive composition according to the present invention can be applied by a hot melt method, a relatively thick pressure-sensitive adhesive layer can be formed with less energy, cost, and time than when the pressure-sensitive adhesive composition is dissolved in a solvent, applied, and dried.

[0066] The type of substrate is not particularly limited, and for example, a nonwoven fabric or a resin film can be used. The adhesive tape may also be a double-sided adhesive tape having adhesive layers composed of an adhesive composition on both sides of the substrate. In this case, the double-sided adhesive tape preferably has adhesive layers of the above-mentioned thickness on both sides of the substrate. A release film may also be attached to the surface of the adhesive layer of the double-sided adhesive tape opposite to the surface that contacts the substrate.

[0067] 2.2. Adhesive Strength The adhesive strength of the adhesive tape to a stainless steel substrate at 23°C based on JIS Z0237 is preferably 10 N / 10 mm or more, more preferably 15 N / 10 mm or more, and even more preferably 17 N / 10 mm or more. Specifically, the adhesive strength may be, for example, 10, 10.5, 11, 11.5, 12, 12.5, 13, 13.5, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, or 25 N / 10 mm, or may be within a range between any two of the values ​​exemplified here. The adhesive strength can be controlled by adjusting the types and amounts of components of the adhesive composition. The adhesive strength can be determined by measuring the 180° peel adhesive strength to the substrate in a 23°C atmosphere based on JIS Z0237 "10. Adhesive Strength."

[0068] 2.3. Constant Load Peel The peel distance of the pressure-sensitive adhesive tape measured by a constant load peel test at 80°C is preferably 50 mm or less, more preferably 45 mm or less, and even more preferably 40 mm or less. The peel distance of the pressure-sensitive adhesive tape may be, for example, 0, 10, 20, 30, 35, 40, 45, or 50 mm, and may be within a range between any two of the values ​​exemplified here. The constant load peel test is performed, for example, as follows: The pressure-sensitive adhesive tape is attached to a polypropylene adherend and treated in an 80°C atmosphere for 10 minutes. Thereafter, a load (100 gf) is applied to the end of the pressure-sensitive adhesive tape in an 80°C atmosphere, perpendicular to the surface of the adherend and in a direction away from the adherend, and the peel distance of the pressure-sensitive adhesive sheet is measured after 30 minutes.

[0069] The present invention will be described in more detail below based on examples, but the present invention should not be construed as being limited to these examples.

[0070] <Preparation of Pressure-Sensitive Adhesive Composition> A tackifier and an antioxidant were added to a kneader kneader heated to 200°C, and the mixture was kneaded at 15 rpm for 10 minutes. Then, a block copolymer was added, and the mixture was kneaded at 15 rpm for a further 100 minutes to obtain a pressure-sensitive adhesive composition. The blending amount (parts by mass) of each component in the pressure-sensitive adhesive composition in the examples and comparative examples is shown in Tables 1 to 3. The viscosity of the first tackifier shown in Tables 1 to 3 is the viscosity at 25°C.

[0071] The block copolymers used in the examples and comparative examples are as follows. Asaprene N521 (manufactured by Asahi Kasei Corporation): SBBS (a styrene-butadiene-based block copolymer in which the butadiene moiety is partially hydrogenated, a styrene-butadiene-butylene-styrene block copolymer), styrene content 25% by mass, diblock content 60% by mass, MFR 2 g / 10 min. In GPC measurement, it has peaks corresponding to the peak top molecular weights of two components (235,000 and 79,000). Tuftec P1500 (manufactured by Asahi Kasei Corporation): SBBS (a styrene-butadiene-based block copolymer in which the butadiene moiety is partially hydrogenated, a styrene content 30% by mass, diblock content 65% by mass, MFR 15 g / 10 min. In GPC measurement, it has peaks corresponding to the peak top molecular weights of three components (125,000, 65,000, 13,000). Tuftec P1083 (manufactured by Asahi Kasei Corporation): SBBS (a styrene-butadiene-butylene-styrene block copolymer, which is a styrene-butadiene block copolymer in which the butadiene moiety is partially hydrogenated), styrene content 20% by mass, diblock content 80% by mass, MFR 10 g / 10 min. GPC measurement shows peaks at the peak top molecular weights of three components (110,000, 50,000, 8,000). Quintac 3421 (manufactured by Zeon Corporation): SIS (styrene-isoprene-styrene block copolymer). Note that the molecular weight in GPC measurement is the polystyrene equivalent molecular weight. The MFR is measured at 200°C and 5 kgf.

[0072] The first tackifiers used in the examples and comparative examples are as follows: YS Resin LP (manufactured by Yasuhara Chemical Co., Ltd.): an aromatic modified terpene resin that is liquid at 23°C, with a flash point of 220°C and a viscosity of 2,000 mPa·s at 25°C; Super Ester A-18 (manufactured by Arakawa Chemical Industries, Ltd.): a rosin ester that is liquid at 23°C and a viscosity of 100,000 mPa·s at 25°C; Ester Gum AT (manufactured by Arakawa Chemical Industries, Ltd.): a rosin ester that is liquid at 23°C and a viscosity of 20,000 to 40,000 mPa·s at 25°C.

[0073] The second tackifiers used in the examples and comparative examples are as follows: YS Resin PX1150N (manufactured by Yasuhara Chemical Co., Ltd.): terpene resin, softening point 115°C; Alcon P-110 (manufactured by Arakawa Chemical Industries, Ltd.): hydrogenated C9 petroleum resin, softening point 110°C; Petrotack 90 (manufactured by Tosoh Corporation): C5 / C9 petroleum resin, softening point 90°C; ESCOREZ1310 (manufactured by ExxonMobil Chemical Co.): C5 petroleum resin, softening point 93°C.

[0074] The third tackifiers used in the examples and comparative examples are as follows: P-140 (manufactured by Arakawa Chemical Industries, Ltd.): hydrogenated C9 petroleum resin, softening point 141°C YS Polystar T-145 (manufactured by Yasuhara Chemical Co., Ltd.): terpene phenol resin, softening point 145°C YS Polystar T-160 (manufactured by Yasuhara Chemical Co., Ltd.): terpene phenol resin, softening point 160°C DS-822 (manufactured by Harima Chemical Group Co., Ltd.): polymerized rosin ester, softening point 165°C

[0075] The antioxidants used in the examples and comparative examples are as follows: Irganox 1010 (manufactured by BASF Japan Ltd.): melting point 110°C Irganox 1726 (manufactured by BASF Japan Ltd.): melting point 28°C Irganox 1035 (manufactured by BASF Japan Ltd.): melting point 63°C Irganox 1024 (manufactured by BASF Japan Ltd.): melting point 225°C Sumilizer GS (manufactured by Sumitomo Chemical Co., Ltd.): melting point 119°C Sumilizer GP (manufactured by Sumitomo Chemical Co., Ltd.): melting point 115°C or higher

[0076] The initial viscosity η0 of the resulting pressure-sensitive adhesive composition at 185°C and the melt viscosity η1 after heating at 185°C for 30 minutes were measured using a rheometer (MCR302, manufactured by Anton Paar) at a shear rate of 10 [1 / s]. The measurement results are shown in Tables 1 to 3.

[0077] <Production of Pressure-Sensitive Adhesive Tape> The prepared pressure-sensitive adhesive composition was heated to 200°C in a melter to melt it, and applied to one side of a substrate (PET film, manufactured by Toray Industries, Inc., product number Lumirror T60 50 µm) using a slot die coater (manufactured by Nordson Chemical) to a thickness of 80 µm to form a pressure-sensitive adhesive layer, thereby producing a pressure-sensitive adhesive tape.

[0078] Using the obtained adhesive tape, the chemiluminescence emission intensity of the adhesive composition was measured 5 minutes after the start of measurement in an atmosphere of 185 ° C. The adhesive tape was punched out to a size of 20 mm wide and 50 mm long, and placed in the sample chamber of a chemiluminescence measuring device (Tohoku Electronics Industry Co., Ltd., CLA-FS4) having a photomultiplier tube as a detection element that had been preheated to 185 ° C., with the adhesive layer facing upward, and measurement was started while air with an oxygen concentration of 20% was sent into the sample chamber at 50 ml / min. The measurement results of the chemiluminescence emission intensity 5 minutes after the start of measurement are shown in Tables 1 to 3.

[0079] <Evaluation> The pressure-sensitive adhesive compositions and pressure-sensitive adhesive tapes of the Examples and Comparative Examples were evaluated as follows.

[0080] (Adhesive Strength) The adhesive strength (180° peel adhesive strength) of the adhesive tape to an SUS adherend was measured in an atmosphere of 23°C. First, the adhesive tape was punched out to a width of 20 mm and a length of 200 mm, and the adhesive surface was attached to the adherend by pressure bonding. Thereafter, the 180° peel strength was measured using a tensile tester in an atmosphere of 23°C at a tensile speed of 300 mm / min. The measurement results are shown in Tables 1 to 3.

[0081] (Constant Load Peel) A constant load peel test was performed at 80°C to measure the peel distance of the adhesive tape. In the constant load peel test, the adhesive tape was attached to a polypropylene adherend and treated in an 80°C atmosphere for 10 minutes, and then a load (100 gf) was applied to the end of the adhesive tape in an 80°C atmosphere, and the peel distance of the adhesive sheet was measured after 30 minutes. The measurement results are shown in Tables 1 to 3.

[0082] (Hot melt coatability) The hot melt coatability of the pressure-sensitive adhesive composition was evaluated. The pressure-sensitive adhesive composition was heated to 200°C in a melter to melt it, and then discharged for 30 minutes using a slot die coater (manufactured by Nordson Corporation). The change in the discharge amount 30 minutes after the start of discharge was evaluated according to the following criteria. The evaluation results are shown in Tables 1 to 3. ○: The discharge amount decreased by less than 10% 30 minutes after the start of discharge compared to when discharged. ×: The discharge amount decreased by 10% or more 30 minutes after the start of discharge compared to when discharged.

[0083] (Evaluation Results) The adhesive compositions of Examples 1 to 17 all showed a small degree of viscosity increase upon prolonged heating and had good hot-melt coatability. Furthermore, the adhesive tapes having adhesive layers formed from the adhesive compositions of Examples 1 to 17 had relatively high adhesive strength and relatively short peel distances in a constant-load peel test, demonstrating good adhesive strength. The adhesive compositions of Comparative Examples 1 and 2 showed a significant increase in viscosity upon heating and had poor hot-melt coatability. In Comparative Examples 1 and 2, the adhesive strength and constant-load peel were not able to be evaluated because the adhesive composition viscosity increase made it difficult to manufacture the adhesive tapes. The adhesive tapes having adhesive layers formed from the adhesive compositions of Comparative Examples 3 and 4 had relatively low adhesive strength and relatively long peel distances in a constant-load peel test.

[0084]

[0085]

[0086]

[0087] Various embodiments of the present invention have been described above, but these are presented as examples and are not intended to limit the scope of the invention. The novel embodiments may be embodied in various other forms, and various omissions, substitutions, and modifications may be made without departing from the spirit of the invention. Such embodiments and modifications are included within the scope and spirit of the invention, and are also included in the scope of the invention and its equivalents as defined in the claims.

Claims

1. A hot melt pressure sensitive adhesive composition comprising a styrene-butadiene block copolymer and a tackifier, wherein the styrene-butadiene block copolymer has a partially hydrogenated butadiene portion, and wherein the chemiluminescence emission intensity 5 minutes after the start of measurement in an atmosphere at 185°C is less than 300,000 count / s.

2. The hot melt pressure sensitive adhesive composition according to claim 1, having a viscosity at 185°C of 10,000 to 100,000 mPa·s.

3. The hot melt pressure sensitive adhesive composition according to claim 1 or 2, which contains an antioxidant.

4. The hot melt pressure sensitive adhesive composition according to claim 3, wherein the antioxidant has a melting point of 60°C or higher.

5. The hot melt pressure sensitive adhesive composition according to claim 1 or 2, wherein the tackifier comprises a first tackifier, and the first tackifier is at least one of a terpene resin that is liquid at 23°C and a rosin ester that is liquid at 23°C.

6. The hot melt adhesive composition according to claim 1 or 2, wherein the tackifier comprises a second tackifier, and the second tackifier has a softening point of 70 to 120°C.

7. The hot melt adhesive composition according to claim 1 or 2, wherein the tackifier comprises a third tackifier, and the third tackifier has a softening point of 140°C or higher.

8. A hot melt adhesive composition according to claim 1 or 2, wherein the tackifier comprises a first tackifier, a second tackifier and a third tackifier, the first tackifier being a terpene resin that is liquid at 23°C, the second tackifier being a terpene resin having a softening point of 70 to 120°C, and the third tackifier being a terpene phenol resin having a softening point of 140°C or higher.

9. The hot melt adhesive composition according to claim 8, comprising 45 to 55 parts by mass of the styrene-butadiene block copolymer, 10 to 20 parts by mass of the first tackifier, 10 to 25 parts by mass of the second tackifier, and 17.5 to 27.5 parts by mass of the third tackifier, based on 100 parts by mass of the hot melt adhesive composition.

10. The hot melt adhesive composition according to claim 9, wherein the content ratio of the first tackifier and the second tackifier in the hot melt adhesive composition is 1:0.5 to 1:1.5 by mass.

11. The hot melt pressure sensitive adhesive composition according to claim 1 or 2, wherein the styrene-butadiene block copolymer has a content of monomer units derived from styrene of 24 mass% or more.

12. The hot melt pressure-sensitive adhesive composition according to claim 1 or 2, wherein the styrene-butadiene block copolymer comprises a component a having a peak top molecular weight of 200,000 or more and 400,000 or less, as measured by GPC, and a component b having a peak top molecular weight of 100,000 or more and less than 200,000.

13. An adhesive tape comprising an adhesive layer containing the hot melt adhesive composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Hot melt adhesive and throwaway product

    JP2014111711A

  • Evaluation method of degradation resistance performance of crosslinked rubber material

    JP2015206743A

  • Partially hydrogenated block copolymer, pressure-sensitive adhesive composition, pressure-sensitive adhesive tape, label, modified asphalt composition, modified asphalt mixture and binder composition for pavement

    JP2020073661A

  • Plastic antioxidant performance evaluating device

    WO2020080085A1

  • Adhesive tape

    WO2023282217A1