Conductive film and display device

The conductive film addresses adhesion and chemical resistance issues by using a segregated silicone-based mold release agent in the resin layer, enhancing substrate adhesion and chemical resistance for long-term transparency and functionality.

WO2024203760A1PCT designated stage expired Publication Date: 2024-10-03TDK CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011127
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-21
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conductive films with mold release agents have issues with resin layer adhesion to the substrate and chemical resistance, leading to void formation and decreased transparency over time.

Method used

A conductive film with a resin layer containing a silicone-based mold release agent, where the mold release agent is segregated to create a surface segregation layer, resulting in a thickness of 5100 nm or less and a silicon-containing secondary ion ratio of 25% or less, enhancing adhesion and chemical resistance.

Benefits of technology

The conductive film achieves improved adhesion to the substrate, preventing void formation and light scattering, and maintains chemical resistance against chemicals, ensuring long-term transparency and functionality as a transparent antenna.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011127_03102024_PF_FP_ABST
    Figure JP2024011127_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a conductive film including a substrate, a resin layer provided on a main surface of the substrate, and a conductive part filled in at least a groove pattern formed in the resin layer. The resin layer is obtained by using a mold release agent including silicon and a resin composition containing a resin. The resin layer has a surface mold release agent segregation layer and a body part provided on a substrate side of the surface mold release agent segregation layer. The surface mold release agent segregation layer has a first surface on an opposite side thereof from the body part, and the body part has a second surface on a substrate side thereof. The thickness of the resin layer is 5100 nm or less. When time-of-flight secondary ion mass spectrometry is performed in the thickness direction of the resin layer, the ratio R defined by formula (1) by using the intensity A1 of silicon-containing secondary ions derived from the mold release agent, on the first surface of the body part and the intensity A2 of silicon-containing secondary ions derived from the mold release agent, on the second surface of the surface mold release agent segregation layer is 25% or less. (1): Ratio R = 100 × A2 / A1
Need to check novelty before this filing date? Find Prior Art

Description

Conductive film and display device

[0001] The present disclosure relates to a conductive film and a display device.

[0002] A conductive film including a transparent antenna having transparency and conductivity is sometimes mounted on the surface of a touch panel or a display. For example, Patent Document 1 below discloses an example of such a conductive film, which is obtained by forming a trench-forming layer on a laminate of a substrate and an underlayer, pressing a mold having convex portions into a resin composition that forms the trench-forming layer by an imprinting method using a mold having convex portions until the convex portions reach the underlayer, forming a mesh-like trench pattern having linear trenches, and filling the trench pattern with conductive portions to form a mesh-like conductive pattern.

[0003] Japanese Patent Application Laid-Open No. 2019-029658

[0004] Incidentally, when a trench pattern is formed in a trench-forming layer by an imprinting method, as in the conductive film of Patent Document 1, after the trench-forming layer is cured to form a resin layer, a release agent may be blended into the resin composition for forming the trench-forming layer in order to improve the releasability of the mold from the resin layer.

[0005] However, when a release agent is blended into the resin composition, the conductive film described in Patent Document 1 has the following problems: The conductive film described in Patent Document 1 has room for improvement in terms of adhesion of the resin layer to the substrate. Furthermore, the conductive film described in Patent Document 1 also has room for improvement in terms of chemical resistance.

[0006] An object of the present disclosure is to provide a conductive film and a display device having a resin layer with excellent adhesion and chemical resistance.

[0007] One aspect of the present disclosure provides a conductive film including: a substrate; a resin layer provided on one or both main surfaces of the substrate; at least a groove pattern formed in the resin layer; and a conductive portion filled in the groove pattern; the resin layer is obtained using a resin composition containing a release agent containing silicon and a resin; the resin layer has a surface release agent segregation layer in which the release agent segregates; and a main portion provided on the substrate side of the surface release agent segregation layer; the surface release agent segregation layer has a first surface opposite to the main portion, and the main portion has a second surface on the substrate side; the resin layer has a thickness of 5100 nm or less; and when time-of-flight secondary ion mass spectrometry is performed on the resin layer in the thickness direction, a ratio R defined by the following formula (1) is 25% or less, using an intensity A1 of silicon-containing secondary ions derived from the release agent on the first surface of the main portion and an intensity A2 of silicon-containing secondary ions derived from the release agent on the second surface of the main portion: Ratio R = 100 × A2 / A1 (1)

[0008] According to this conductive film, a portion of the resin layer provided on one or both main surfaces of the substrate is a surface release agent segregation layer where the release agent segregates, and the remaining portion is a main body portion. By setting the ratio R, expressed by the above formula (1), of the intensity of silicon-containing secondary ions derived from the release agent on the second surface of the main body portion relative to the first surface of the surface release agent segregation layer to 25% or less, the amount of release agent on the second surface side of the main body portion can be reduced compared to when the ratio R is greater than 25%. Furthermore, by setting the thickness of the resin layer to 5100 nm or less, the adhesive area between the resin layer and the substrate per unit thickness can be increased. Therefore, the conductive film of the present disclosure has excellent adhesion of the resin layer to the substrate. Meanwhile, by setting the ratio R to 25% or less, the resin is protected from chemicals even when the resin layer comes into contact with chemicals. Therefore, the conductive film of the present disclosure also has excellent chemical resistance.

[0009] Another aspect of the present disclosure provides a display device comprising an image display unit and a conductive film disposed on the image display unit, the conductive film being the conductive film described above. Because the conductive film has excellent adhesion to the resin layer, the formation of voids between the substrate and the resin layer, which can cause light scattering, is suppressed over a long period of time, thereby suppressing a decrease in transmittance due to the voids. Furthermore, because the conductive film also has excellent chemical resistance, even if the conductive film comes into contact with chemicals, deterioration of the resin due to the chemicals is suppressed, and a decrease in the transparency of the conductive film due to resin deterioration is suppressed over a long period of time. Therefore, the display device of the present disclosure can suppress a decrease in visibility of the image display unit through the conductive film over a long period of time.

[0010] In the conductive film, the thickness of the surface release agent segregation layer is preferably 30% or less of the thickness of the resin layer, in which case the conductive film is superior in adhesion to the resin layer and chemical resistance compared to a case in which the thickness of the surface release agent segregation layer exceeds 30% of the thickness of the resin layer.

[0011] In the conductive film, the ratio R is preferably 20% or less. In this case, the conductive film is superior in adhesiveness of the resin layer and chemical resistance compared to a case where the ratio R exceeds 20%.

[0012] In the conductive film, the substrate may have an underlayer in contact with the resin layer, and the underlayer may contain at least one metal selected from the group consisting of palladium, copper, nickel, and aluminum.

[0013] In the conductive film, the groove pattern may include a plurality of linear trenches that intersect with each other.

[0014] In the conductive film, the groove pattern may be a mesh pattern.

[0015] The conductive film has excellent adhesion to the resin layer, so that the formation of voids between the substrate and the resin layer, which cause light scattering, is suppressed for a long period of time, and the decrease in transmittance due to the voids is suppressed. Furthermore, the conductive film has excellent chemical resistance, so that even if the conductive film comes into contact with chemicals, the deterioration of the resin due to the chemicals is suppressed, and the decrease in transparency of the conductive film due to the resin deterioration is suppressed for a long period of time. Therefore, the conductive film is useful when used in a transparent antenna.

[0016] In the present disclosure, the term "surface release agent segregation layer" refers to a region in which, when time-of-flight secondary ion mass spectrometry is performed on the resin layer in its thickness direction, the intensity of silicon-containing secondary ions derived from the release agent is maintained within a range of −75% to +75% of the intensity of silicon-containing secondary ions on the first surface.

[0017] According to the present disclosure, a conductive film and a display device are provided which have excellent adhesiveness and chemical resistance of a resin layer.

[0018] Fig. 2 is a plan view showing a conductive film according to an embodiment of the present disclosure. Fig. 3 is a cross-sectional view taken along line II-II in Fig. 1. Fig. 4 is an enlarged plan view of the vicinity of an intersection where two linear trenches and two linear portions of a conductive portion intersect with each other. Fig. 5 is a partially enlarged view of Fig. 2. Fig. 6 is a cross-sectional view showing an embodiment of a display device according to the present disclosure. Fig. 7 is a graph showing the relationship between the depth from the first surface and the strength of silicon-containing secondary ions derived from the release agent according to Example 1.

[0019] Hereinafter, embodiments of the present disclosure will be described in detail.

[0020] <Conductive Film> First, an embodiment of a conductive film according to the present disclosure will be described with reference to the drawings. Fig. 1 is a plan view showing a conductive film according to one embodiment of the present disclosure. Fig. 2 is a cross-sectional view taken along line II-II in Fig. 1. Fig. 3 is an enlarged plan view of the vicinity of an intersection where two linear trenches and two linear portions of a conductive portion intersect with each other. Fig. 4 is a partially enlarged view of Fig. 2.

[0021] As shown in FIGS. 1 to 4 , the conductive film 20 is primarily composed of a substrate 15, a first resin layer 30 provided on one main surface 15S of the substrate 15, a groove pattern 7 formed in the first resin layer 30, and conductive portions 5 filled in the groove pattern 7. The first resin layer 30 is obtained using a resin composition containing a silicone-containing release agent and a resin. The first resin layer 30 also has a surface release agent segregation layer 31 in which the release agent segregates, and a main body portion 32 provided on the substrate 15 side of the surface release agent segregation layer 31. The surface release agent segregation layer 31 has a first surface 31a on the side opposite the main body portion 32, and the main body portion 32 has a second surface 32a on the substrate 15 side. The thickness of the first resin layer 30 is 5100 nm or less. In the conductive film 20, when time-of-flight secondary ion mass spectrometry (TOF-SIMS) is performed on the first resin layer 30 in the thickness direction Y, the ratio R defined by the following formula (1) using the intensity A1 of silicon-containing secondary ions derived from the release agent on the first surface 31a of the surface release agent segregation layer 31 and the intensity A2 of silicon-containing secondary ions derived from the release agent on the second surface 32a of the main body portion 32 is 25% or less: Ratio R=100×A2 / A1 (1)

[0022] The substrate 15 has a film-like base material 1 and an intermediate layer 11 provided between the base material 1 and a first resin layer 30. The intermediate layer 11 includes a second resin layer 12 and an underlayer 13, in this order, from the base material 1 side. The conductive film 20 may further include a protective layer (not shown) on a main surface 1a of the base material 1 opposite to the first resin layer 30 and the intermediate layer 11.

[0023] In the conductive film 20, as shown in FIG. 3, a mesh-like groove pattern 7 is formed by a plurality of linear trenches 7a extending along two directions A and B, respectively, intersecting with each other at intersections X.

[0024] The conductive portion 5 has a portion (linear portion) 5a provided in the linear trench 7a. The conductive portion 5 in the groove pattern 7 having the trench 7a also forms a mesh-like pattern.

[0025] According to this conductive film 20, a portion of the first resin layer 30 provided on one main surface 15S of the substrate 15 is a surface release agent segregation layer 31 where the release agent segregates, and the remaining portion is a main body portion 32. By setting the ratio R, expressed by the above formula (1), of the intensity of silicon-containing secondary ions derived from the release agent on the second surface 32a of the main body portion 32 relative to the first surface 31a of the surface release agent segregation layer 31 to 25% or less, the amount of release agent on the second surface 32a of the main body portion 32 can be reduced compared to when the ratio R is greater than 25%. Furthermore, by setting the thickness of the first resin layer 30 to 5100 nm or less, the adhesive area per unit thickness between the first resin layer 30 and the substrate 15 can be increased. Therefore, the conductive film 20 has excellent adhesion of the first resin layer 30 to the substrate 15. On the other hand, by setting the ratio R to 25% or less, the resin in the first resin layer 30 is protected from chemicals even when the first resin layer 30 comes into contact with chemicals. Therefore, the conductive film 20 also has excellent chemical resistance.

[0026] Because the conductive film 20 has excellent adhesion to the first resin layer 30, the formation of voids between the substrate 15 and the first resin layer 30, which can cause light scattering, is suppressed for a long period of time, and a decrease in transmittance due to voids is suppressed. Furthermore, because the conductive film 20 has excellent chemical resistance, even if the conductive film 20 comes into contact with chemicals, deterioration of the resin due to the chemicals is suppressed, and a decrease in the transparency of the conductive film 20 due to resin deterioration is suppressed for a long period of time. Therefore, the conductive film 20 is useful when used in a transparent antenna. In particular, the conductive portion 5 having a mesh-like pattern can function well, for example, as a radiating element of an antenna.

[0027] The substrate 1, the first resin layer 30, the second resin layer 12, the underlayer 13, the groove pattern 7, the conductive portion 5, and the protective layer will be described in detail below.

[0028] (Substrate) The substrate 1 may be a light-transmitting substrate. The light-transmitting substrate has a degree of light transparency required when the conductive film 20 is incorporated into a display device, for example. Specifically, the total light transmittance of the light-transmitting substrate may be 90 to 100%. The haze of the light-transmitting substrate may be 0 to 5%.

[0029] The light-transmitting substrate used as the substrate 1 may be, for example, a transparent resin film, examples of which include films of polyethylene terephthalate (PET), polycarbonate (PC), polyethylene naphthalate (PEN), cycloolefin polymer (COP), or polyimide (PI). Alternatively, the light-transmitting substrate may be a glass substrate.

[0030] The thickness of the substrate 1 may be 1 μm or more, 10 μm or more, or 20 μm or more, and may be 500 μm or less, 200 μm or less, or 100 μm or less.

[0031] (First Resin Layer) The first resin layer 30 is obtained using a resin composition containing a resin and a release agent containing silicon. The first resin layer 30 may be made of the above-mentioned resin composition, or may be made of a cured product of the above-mentioned resin composition. The total light transmittance of the first resin layer 30 may be 90 to 100%. The haze of the first resin layer 30 may be 0 to 5%.

[0032] The resin in the resin composition may be a curable resin composition or a cured product thereof. Examples of the curable resin include acrylic resins, amino resins, cyanate resins, isocyanate resins, polyimide resins, epoxy resins, oxetane resins, polyester resins, allyl resins, phenolic resins, benzoxazine resins, xylene resins, ketone resins, furan resins, COPNA resins, silicon resins, dicyclopentadiene resins, benzocyclobutene resins, episulfide resins, ene-thiol resins, polyazomethine resins, polyvinylbenzyl ether compounds, acenaphthylene, and ultraviolet-curable resins containing functional groups that undergo a polymerization reaction under ultraviolet light, such as unsaturated double bonds, cyclic ethers, and vinyl ethers.

[0033] Examples of silicone-containing release agents include release agents having ultraviolet-curable or heat-curable functional groups, such as acrylic-modified reactive silicone oil and epoxy-modified reactive silicone oil, and release agents having functional groups capable of crosslinking with the curable resin. Among these, release agents having functional groups capable of crosslinking with the curable resin are preferred. In this case, the strength and chemical resistance of the first resin layer 30 are further improved by crosslinking with the curable resin. One type of release agent may be used alone, or two or more types may be used in combination.

[0034] The content of the release agent in the resin composition is not particularly limited, but is preferably 30% by mass or less, more preferably 20% by mass or less, and particularly preferably 15% by mass or less. When the content of the release agent in the resin composition is 30% by mass or less, the adhesion of the first resin layer 30 to the substrate 15 can be further improved compared to when the content of the release agent in the resin composition exceeds 30% by mass. However, the content of the release agent in the resin composition may be greater than 0% by mass, but is preferably 1% by mass or more, and more preferably 2% by mass or more. When the content of the release agent in the resin composition is 1% by mass or more, the shape of the groove pattern 7 is less likely to be distorted, and a better appearance can be obtained, compared to when the content of the release agent in the resin composition is less than 1% by mass.

[0035] The ratio R may be 25% or less, preferably 22% or less or 21% or less. In this case, the conductive film 20 is superior in adhesion and chemical resistance of the first resin layer 30 compared to when the ratio R exceeds 25%. The ratio R is preferably 20% or less, more preferably 18% or less, even more preferably 15% or less, and particularly preferably 10% or less. In this case, the conductive film 20 is superior in adhesion and chemical resistance of the first resin layer 30 compared to when the ratio R exceeds 20%. The ratio R may be 5% or less, or may be 2% or less. The ratio R may be 5% or more, 10% or more, 13% or more, or 15% or more. In the above formula (1), A1 and A2 represent the intensities of silicon-containing secondary ions derived from the release agent on the first surface 31a and silicon-containing secondary ions derived from the release agent on the second surface 32a of the main body 32, respectively. Here, examples of silicon-containing secondary ions include SiC. 3 H 9 + , SiO + Examples include:

[0036] The thickness of the first resin layer 30 may be 5100 nm or less. In this case, the adhesion of the first resin layer 30 to the substrate 15 can be further improved compared to when the thickness of the first resin layer 30 exceeds 5100 nm. From the viewpoint of further improving the adhesion of the first resin layer 30 to the substrate 15, the thickness of the first resin layer 30 may be 5000 nm or less, 4500 nm or less, 4000 nm or less, 3500 nm or less, 3000 nm or less, 2500 nm or less, 2000 nm or less, 1500 nm or less, or 1000 nm or less. The thickness of the first resin layer 30 is preferably 1000 nm or more. In this case, compared to when the thickness of the first resin layer 30 is less than 1000 nm, the depth of the trench 7 a is greater and the volume resistivity of the conductive portion 5 is further reduced, thereby further improving the conductivity of the conductive film 20. From the viewpoint of further improving the conductivity of the conductive film 20, the thickness of the first resin layer 30 may be 2000 nm or more, 2500 nm or more, 3000 nm or more, 3500 nm or more, or 4000 nm or more.

[0037] The thickness of the surface release agent segregation layer 31 is not particularly limited as long as it is smaller than the thickness of the first resin layer 30, but is preferably 30% or less of the thickness of the first resin layer 30. In this case, the conductive film 20 is superior in adhesion and chemical resistance to the first resin layer 30 compared to when the thickness of the surface release agent segregation layer 31 exceeds 30% of the thickness of the first resin layer 30. The thickness of the surface release agent segregation layer 31 may be 20% or less, or 10% or less. However, the thickness of the surface release agent segregation layer 31 may be greater than 0 nm, but is preferably 5 nm or more, and more preferably 10 nm or more. In this case, the release component can be uniformly segregated on the surface of the first resin layer 30 compared to when the thickness of the first resin layer 30 is less than 5 nm, resulting in better releasability when the trench mold is removed, and therefore reducing damage to the first resin layer 30 when the mold is removed. The thickness of the surface release agent segregation layer 31 may be 50 nm or more, or 100 nm or more.

[0038] (Second Resin Layer) The second resin layer 12 is provided between the substrate 1 and the underlayer 13. This can improve the adhesion between the substrate 1 and the underlayer 13.

[0039] The second resin layer 12 may be a layer containing a resin and an inorganic filler. An example of the resin constituting the second resin layer 12 is an acrylic resin. An example of the inorganic filler is silica.

[0040] The thickness of the second resin layer 12 may be, for example, 5 nm or more, 100 nm or more, 200 nm or more, 500 nm or more, or 1 μm or more, and may be 10 μm or less, 5 μm or less, or 2 μm or less.

[0041] (Underlayer) The underlayer 13 is a layer provided for forming the conductive portion 5 by electroless plating or the like. The underlayer 13 may be a layer containing a catalyst and a resin. The underlayer 13 may be a single layer or a laminate of multiple layers. The resin may be a cured product of a curable resin composition. Examples of the curable resin contained in the curable resin composition include amino resins, cyanate resins, isocyanate resins, polyimide resins, epoxy resins, oxetane resins, polyester resins, allyl resins, phenolic resins, benzoxazine resins, xylene resins, ketone resins, furan resins, COPNA resins, silicon resins, dicyclopentadiene resins, benzocyclobutene resins, episulfide resins, ene-thiol resins, polyazomethine resins, polyvinylbenzyl ether compounds, acenaphthylene, and ultraviolet-curable resins containing functional groups that undergo a polymerization reaction under ultraviolet light, such as unsaturated double bonds, cyclic ethers, and vinyl ethers.

[0042] The catalyst contained in the underlayer 13 may be an electroless plating catalyst. The electroless plating catalyst may be at least one metal selected from the group consisting of Pd, Cu, Ni, Al, Co, Au, Ag, Pd, Rh, Pt, In, and Sn, at least one metal selected from the group consisting of Pd, Cu, Ni, and Al, at least one metal selected from the group consisting of Pd, Cu, and Ni, or Pd. The catalyst may be one type alone or a combination of two or more types. Typically, the catalyst is dispersed in the resin as catalyst particles.

[0043] The catalyst content in the underlayer 13 may be 3 mass% or more, 4 mass% or more, or 5 mass% or more, based on the total amount of the underlayer 13, and may be 100 mass% or less, 50 mass% or less, or 25 mass% or less.

[0044] The thickness of the underlayer 13 may be 5 nm or more, 10 nm or more, or 30 nm or more, and may be 500 nm or less, 300 nm or less, or 150 nm or less.

[0045] (Trough Pattern) In the groove pattern 7, the angle between two intersecting linear trenches 7a does not need to be 90 degrees, but can be, for example, in the range of 40 degrees to 140 degrees.

[0046] (Conductive Portion) The conductive portion 5 is provided, together with the groove pattern 7 , over a partial region of the first resin layer 30 .

[0047] The conductive portion 5 may contain a metal as a conductive material. The conductive portion 5 may contain at least one metal selected from copper, nickel, cobalt, palladium, silver, gold, platinum, and tin, or may contain copper. The conductive portion 5 may be a metal plating formed by a plating method. The conductive portion 5 may further contain a non-metallic element such as phosphorus, as long as appropriate conductivity is maintained.

[0048] The aspect ratio of the conductive portion 5 may be 0.1 or more, 0.5 or more, or 1.0 or more. By setting the aspect ratio of the conductive portion 5 within the above range, the conductivity of the conductive portion 5 can be further increased. The aspect ratio of the conductive portion 5 may be 10.0 or less, 7.0 or less, or 4.0 or less. By setting the aspect ratio of the conductive portion 5 within the above range, the difference in transmittance depending on the angle of incidence of light with respect to the surface 31a of the first resin layer 30 opposite the substrate 1 can be reduced. The aspect ratio of the conductive portion 5 refers to the ratio of the thickness of the conductive portion 5 to the width of the conductive portion 5 (thickness / width).

[0049] The conductive portion 5 may be a laminate composed of multiple layers. For example, the conductive portion 5 may be composed of a first metal layer and a second metal layer formed in this order on the substrate 1. The first metal layer may contain nickel. The second metal layer may contain copper. The thickness of the first metal layer may be, for example, 5 nm or more, 10 nm or more, or 50 nm or more, or may be 500 nm or less, 200 nm or less, or 100 nm or less.

[0050] The conductive film 20 may further include a blackening layer. The blackening layer may be provided between the viewer's eye of the conductive film 20 and the conductive portion 5. For example, if the viewer's eye is located on the first resin layer 30 side of the substrate 1, the blackening layer may be provided on the conductive portion 5 on the side opposite the substrate 1. If the viewer's eye is located on the main surface 1a of the substrate 1 opposite the first resin layer 30, the blackening layer may be provided on the conductive portion 5 on the substrate 1 side. In this case, for example, the entire intermediate layer 11 may be a blackening layer, or only a portion of the intermediate layer 11 (the second resin layer 12 or the underlayer 13) may be a blackening layer. The blackening layer may contribute to improving the visibility of a display device incorporating the conductive film 20. The blackening layer may be a layer similar to the first metal layer, for example, a layer containing copper and nickel. In this case, the nickel content of the blackening layer may be 15% by mass or more and 60% by mass or less based on the total amount of copper and nickel. The thickness of the blackened layer may be, for example, 300 nm to 400 nm. The blackened layer may be a layer formed by treating the conductive portion 5 with a treatment liquid containing Pd.

[0051] (Protective Layer) The substrate 15 or the conductive film 20 may further include a protective layer. The protective layer may be provided so as to cover the conductive portion 5, or may be provided so as to cover the main surface 1a of the base material 1 opposite to the first resin layer 30. By providing the protective layer so as to cover the conductive portion 5, scratches on the conductive portion 5 are suppressed, and by providing the protective layer so as to cover the main surface 1a of the base material 1 opposite to the first resin layer 30, scratches on the base material 1 are suppressed. The protective layer may be a layer similar to the second resin layer 12. The thickness of the protective layer may be 5 nm or more, 50 nm or more, or 500 nm or more, and may be 10 μm or less, 5 μm or less, or 2 μm or less.

[0052] <Method for Manufacturing Conductive Film> The conductive film 20 can be manufactured by a method including pattern formation by, for example, imprinting. One example of a method for manufacturing the conductive film 20 includes the steps of: preparing a substrate 15 having a second resin layer 12 and an underlayer 13, in this order, on one main surface of a base material 1; forming a trench-forming layer on the underlayer 13 of the substrate 15; pressing a mold having linear protrusions into the trench-forming layer and then withdrawing the mold from the first resin layer 30 to form a first resin layer 30 having a groove pattern 7 including linear trenches 7 a; and forming conductive portions 5 including linear portions 5 a provided in the linear trenches 7 a by a plating method including growing a metal plating from the underlayer 13 exposed in the trenches 7 a. When the trench-forming layer is a layer containing a thermosetting resin composition as the resin composition, the trench-forming layer may be thermally cured while the mold is pressed into the trench-forming layer to form the first resin layer 30. When the trench forming layer contains a photocurable resin composition, the trench forming layer may be irradiated with ultraviolet light while the mold is pressed into the trench forming layer, thereby curing the trench forming layer and forming the first resin layer 30.

[0053] The pressure applied to the trench forming layer by the convex portions of the mold used in the imprint method may be 2.0 MPa or less, or 1.5 MPa or less.

[0054] After the trench 7a is formed by the imprint method, if a portion of the first resin layer 30 or the second resin layer 12 remains at the bottom of the trench 7a, it may be removed before forming the conductive portion 5. However, when the trench 7a is formed by the imprint method, the conductive portion 5 having good conductivity can be efficiently formed by plating without the need to remove the remaining resin layer.

[0055] Formation of the conductive portion 5 by plating may include, for example, a step of forming a seed layer on the underlayer 13 by electroless plating and a step of forming a Cu plating on the seed layer by electroless plating. In this case, the seed layer may be the first metal layer, and the Cu plating may be the second metal layer.

[0056] <Display Device> Next, a display device according to the present disclosure will be described. The display device according to the present disclosure may include the conductive film 20 as, for example, a planar transparent antenna. The display device may be, for example, a liquid crystal display device or an organic EL display device.

[0057] An embodiment of the display device of the present disclosure will be described with reference to FIG. 5 . FIG. 5 is a cross-sectional view showing an example of a display device incorporating a conductive film. The display device 100 shown in FIG. 5 includes an image display unit 10 having an image display area 10S, a conductive film 20, a polarizing plate 35, and a cover glass 40. The conductive film 20, the polarizing plate 35, and the cover glass 40 are stacked in this order from the image display unit 10 side on the image display area 10S side of the image display unit 10. The configuration of the display device is not limited to the configuration shown in FIG. 5 and can be appropriately modified as needed. For example, the polarizing plate 35 may be provided between the image display unit 10 and the conductive film 20. The image display unit 10 may be, for example, a liquid crystal display unit. The polarizing plate 35 and the cover glass 40 may be those typically used in display devices. The polarizing plate 35 and the cover glass 40 are not necessarily provided.

[0058] The present disclosure is not limited to the above-described embodiment. For example, in the above-described embodiment, the substrate 15 includes the intermediate layer 11 and the first resin layer 30 on one main surface 1 b of the base material 1, but may further include at least one of the intermediate layer 11 and the first resin layer 30 on the main surface 1 a of the base material 1 opposite to the one main surface 1 b.

[0059] Furthermore, in the above embodiment, the groove pattern 7 and the conductive portion 5 are provided over a portion of the first resin layer 30, but they may be provided over the entire area of ​​the first resin layer 30 or the main surface of the substrate 1. Furthermore, in the above embodiment, the intermediate layer 11 is provided so as to cover the entire main surface 1b of the substrate 1, but the intermediate layer 11 may be provided so as to cover a portion of the main surface 1b of the substrate 1. In this case, the remaining area of ​​the main surface 1b of the substrate 1 is not covered by the intermediate layer 11, but is directly covered by the first resin layer 30. In this case, from the viewpoint of suppressing a step between the film on the portion of the main surface 1b of the substrate 1 and the film on the remaining area of ​​the main surface 1b of the substrate 1, it is preferable that the thickness of the intermediate layer 11 be 10% or less of the thickness of the first resin layer 30.

[0060] In the above embodiment, the groove pattern 7 is formed only in the first resin layer 30, but the groove pattern 7 may be formed across the first resin layer 30 and the intermediate layer 11, or across the first resin layer 30, the intermediate layer 11, and the substrate 1. The gist of the present disclosure is as follows. [1] A conductive film comprising: a substrate; a resin layer provided on one or both main surfaces of the substrate; at least a groove pattern formed in the resin layer; and a conductive portion filled in the groove pattern; wherein the resin layer is obtained using a resin composition containing a release agent containing silicon and a resin; the resin layer has a surface release agent segregation layer in which the release agent segregates, and a main portion provided on the substrate side of the surface release agent segregation layer; the surface release agent segregation layer has a first surface opposite to the main portion, and the main portion has a second surface on the substrate side; the resin layer has a thickness of 5100 nm or less; and when time-of-flight secondary ion mass spectrometry is performed on the resin layer in its thickness direction, a ratio R defined by the following formula (1) using an intensity A1 of silicon-containing secondary ions derived from the release agent on the first surface of the surface release agent segregation layer and an intensity A2 of silicon-containing secondary ions derived from the release agent on the second surface of the main portion is 25% or less. Ratio R = 100 × A2 / A1 (1). [2] The conductive film according to [1], wherein the thickness of the surface release agent segregation layer is 30% or less of the thickness of the first resin layer. [3] The conductive film according to [1] or [2], wherein the ratio R is 20% or less. [4] The conductive film according to any one of [1] to [3], wherein the substrate has an underlayer in contact with the resin layer, and the underlayer contains at least one metal selected from the group consisting of palladium, copper, nickel, and aluminum. [5] The conductive film according to any one of [1] to [4], wherein the groove pattern includes a plurality of linear trenches intersecting each other. [6] The conductive film according to [5], wherein the groove pattern is a mesh pattern. [7] The conductive film according to any one of [1] to [6], wherein the conductive film is used for a transparent antenna.[8] A display device comprising: an image display unit; and a conductive film provided on the image display unit, wherein the conductive film is the conductive film according to any one of [1] to [7].

[0061] The present invention will be described in detail below using examples, but the present invention is not limited to these examples. <Preparation of composition for forming base layer> A composition for forming a base layer containing 0.2 mass% Pd particles and an acrylic resin, which is a UV-curable resin, was prepared. <Preparation of composition for forming hard coat layer> A composition for forming a hard coat layer containing 5 mass% Si particles and an acrylic resin, which is a UV-curable resin, was prepared.

[0062] Example 1 First, the hard coat layer-forming composition prepared as described above was applied to a transparent substrate, a cycloolefin polymer (COP) film (thickness: 100 μm), using a bar coater. The coating film was heated to 100°C and cured by ultraviolet irradiation to form a hard coat layer (thickness: 300 nm). Then, the undercoat layer-forming composition prepared as described above was applied to the hard coat layer using a bar coater. The coating film was heated to 100°C and cured by ultraviolet irradiation to form an undercoat layer (thickness: 60 nm). A substrate was thus obtained. Then, a resin layer-forming resin composition consisting of resin composition A, as shown in Table 1, was applied to the undercoat layer of the substrate to form a trench-forming layer. In this case, resin composition A was a resin composition obtained by adding a release agent (product name "X-2-2445", manufactured by Shin-Etsu Chemical Co., Ltd.) to resin composition B (product name "EL1500", manufactured by Showa Denko Materials Co., Ltd., release agent content: 2% by mass), and the amount of additives in resin composition A was adjusted so that the total content of the release agent was 5% by mass as shown in Table 1.

[0063] On the other hand, a Ni mold with 1 μm-wide convex portions forming a mesh-like pattern was prepared. This mold was pressed against the trench-forming layer, and the tips of the mold's convex portions reached the base layer. In this state, the trench-forming layer was cured by ultraviolet irradiation. As a result, the trench-forming layer became a resin layer with a thickness of 2015 nm, and a trench with a bottom surface that exposed the base layer was formed in the resin layer. The trench width was 1 μm and the depth was 2015 nm.

[0064] A laminate having a trench-forming layer forming a trench was immersed in an alkaline degreasing solution containing a surfactant for 5 minutes. The laminate was then removed from the degreasing solution and washed with pure water. The washed laminate was then immersed in an electroless plating solution containing nickel sulfate and sodium hypophosphite for 3 minutes to grow a metal plating as a seed layer (50 nm thick) composed of Ni and P from the base layer exposed at the bottom of the trench. The laminate was then removed from the electroless plating solution and washed with pure water. The laminate with the seed layer formed was then immersed in an aqueous solution containing Pd for 5 minutes and then washed with pure water to allow Pd particles as a catalyst to be adsorbed onto the seed layer. The laminate was then immersed in an electroless plating solution containing copper sulfate and formalin for 15 minutes to grow a Cu plating (top metal plating layer) filling the trench on the seed layer. The laminate was removed from the electroless plating solution and washed with pure water and dried at 80°C for 3 minutes to form a mesh-like pattern, resulting in a conductive film having a conductive pattern layer composed of a seed layer and Cu plating.

[0065] The resin layer of the conductive film thus obtained was subjected to depth analysis using a time-of-flight secondary ion mass spectrometer (product name "TOF.SIMS 5", manufactured by ION-TOF Inc.) to determine the amount of SiC in the thickness direction of the resin layer. 3 H 9 + The intensity of the secondary ions (silicon-containing ions derived from the release agent) (hereinafter referred to as "secondary ion intensity") was measured. At this time, sputtering was performed using a gas cluster ion beam (GCIB), and the ions used for analysis were Bi (primary ions: Bi +) was used. The results are shown in FIG. 6. In FIG. 6, the vertical axis represents the secondary ion intensity, and the horizontal axis represents the depth from the first surface, which is the outermost surface of the resin layer. P represents the surface release agent segregation layer, and Q represents the main body portion. Table 1 also shows the thickness (nm) of the surface release agent segregation layer, the secondary ion intensity A1 at the first surface, which is the outermost layer, the secondary ion intensity A2 at the second surface, which is the main body portion, and the ratio R (= 100 × A2 / A1).

[0066] [Examples 2 to 5 and Comparative Examples 1 to 3] Conductive films were obtained in the same manner as in Example 1, except that the type of resin composition, the content of the release agent, the total thickness of the resin layer, the thickness (nm) of the surface release agent segregation layer, the secondary ion strength A1 on the first side, the secondary ion strength A2 on the second side, and the ratio R (= 100 × A2 / A1) were set as shown in Table 1. Resin composition C was a resin composition (release agent content: 5% by mass) manufactured by Chang Sung Sheet Co., Ltd., with the product name "AM11J5."

[0067] <Evaluation of Adhesion> The adhesiveness of the resin layer to the substrate was evaluated for the conductive films obtained in Examples 1 to 5 and Comparative Examples 1 to 3 by a cross-cut test. The cross-cut test was performed in accordance with JIS K5400. First, 11 cuts were made in the resin layer of the conductive films obtained in Examples 1 to 5 and Comparative Examples 1 to 3 at 1 mm intervals along both the vertical and horizontal directions to form a grid of 100 squares. Cellophane tape was then applied to the cut areas. The applied cellophane tape was peeled off, and the peeling state of the 100 squares was visually observed. The results were evaluated on a six-point scale: 0, 1, 2, 3, 4, and 5. A score of 0 indicates higher adhesiveness, and scores from 0 to 5 indicate gradually lower adhesiveness. The adhesiveness evaluation results are shown in Table 1.

[0068] <Evaluation of Chemical Resistance> The conductive films obtained in Examples 1 to 5 and Comparative Examples 1 to 3 were immersed in a 1% aqueous sodium hydroxide solution at 25°C as an alkaline solution for 3 minutes, and then the surface of the resin layer was observed at 10x magnification using an optical microscope to evaluate chemical resistance. The evaluation criteria for chemical resistance were as follows. The results of chemical resistance are shown in Table 1. (Evaluation criteria) ⊚: The number of circular defects in the field of view of the microscope is 0. ◯: The number of circular defects in the field of view of the microscope is more than 0 but less than 5. ×: The number of circular defects in the field of view of the microscope is 5 or more.

[0069]

[0070] 5...conductive portion, 7...groove pattern, 7a...trench, 10...image display portion, 13...underlying layer, 15...substrate, 15S...main surface, 20...conductive film, 30...first resin layer (resin layer), 31...surface release agent segregation layer, 31a...first surface, 32...main body portion, 32a...second surface, 100...display device, X...intersection portion, Y...thickness direction of the first resin layer.

Claims

1. A conductive film comprising: a substrate; a resin layer provided on one or both main surfaces of the substrate; at least a groove pattern formed in the resin layer; and a conductive portion filled in the groove pattern, the resin layer being obtained using a resin composition containing a release agent containing silicon and a resin, the resin layer having a surface release agent segregation layer in which the release agent segregates, and a main body portion provided on the substrate side of the surface release agent segregation layer, the surface release agent segregation layer having a first surface opposite the main body portion, and the main body portion having a second surface on the substrate side, the resin layer having a thickness of 5,100 nm or less, and when time-of-flight secondary ion mass spectrometry is performed on the resin layer in its thickness direction, a ratio R defined by the following formula (1) using an intensity A1 of silicon-containing secondary ions derived from the release agent on the first surface of the surface release agent segregation layer and an intensity A2 of silicon-containing secondary ions derived from the release agent on the second surface of the main body portion is 25% or less. Ratio R = 100 × A2 / A1 ... (1) 2. The conductive film according to claim 1, wherein the thickness of said surface release agent segregation layer is 30% or less of the thickness of said resin layer.

3. The conductive film according to claim 1, wherein the ratio R is 20% or less.

4. The conductive film according to claim 1, wherein the substrate has an underlayer in contact with the resin layer, and the underlayer contains at least one metal selected from the group consisting of palladium, copper, nickel and aluminum.

5. The conductive film of claim 1, wherein the groove pattern comprises a plurality of linear trenches that intersect with each other.

6. The conductive film according to claim 5, wherein the groove pattern is a mesh-like pattern.

7. The conductive film according to claim 1, which is used for a transparent antenna.

8. A display device comprising: an image display section; and a conductive film provided on said image display section, said conductive film being the conductive film according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Conductive substrate, electronic device, and display device

    JP2019029658A

  • Method of manufacturing fine pattern

    JP2011159924A

  • Electroconductive film and display device

    WO2022138000A1