Polymer composition and rubber product
The polymer composition, with a conjugated diene polymer and aromatic olefin-containing raw material polymer, addresses the balance of grip and breaking strength in tires by optimizing structural units and additives, resulting in enhanced performance in tire products.
Patent Information
- Application Number
- PCT/JP2024/011139
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-03
AI Technical Summary
Existing rubber compositions for tires face challenges in balancing grip properties and breaking strength, as described in Patent Documents 1 and 2, which have room for improvement in this aspect.
A polymer composition is developed containing a conjugated diene polymer with specific structural units and a raw material component polymer, including aromatic olefins, which is formulated to have a specific content of aromatic vinyl compounds and nitrogen-containing groups, along with a hydrocarbyloxysilyl group, to enhance grip and breaking strength.
The polymer composition achieves high grip properties and breaking strength in tire products, specifically in tires, tire treads, and sidewalls, by optimizing the content and structure of the conjugated diene polymer and raw material component polymer.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Polymer compositions and rubber products
[0001] The present invention relates to a polymer composition and a rubber product formed using the polymer composition.
[0002] Traditionally, tires have been manufactured from rubber compositions containing vulcanizing agents, fillers such as carbon black and silica, antioxidants and waxes that prevent deterioration, and each of these components has been improved.
[0003] In recent years, various performance characteristics, such as grip and rolling resistance, have been required of tires. For example, Patent Document 1 describes a rubber composition containing a hydrogenated dicyclopentadiene (DCPD)-based petroleum resin. In Patent Document 1, it has been found that compositions containing specific hydrogenated DCPD-based resins have high grip and low rolling resistance. Furthermore, Patent Document 2 describes a rubber composition for a tire innerliner containing a C5, C9, or hydrogenated DCPD hydrocarbon resin. It has been found that compositions comprising at least one of DCPD-based polymers, cyclopentadiene (CPD)-based polymers, DCPD-styrene copolymers, C5 homopolymer and copolymer resins, C5-styrene copolymer resins, terpene homopolymer or copolymer resins, pinene homopolymer or copolymer resins, C9 homopolymer and copolymer resins, C5 / C9 copolymer resins, alpha-methylstyrene homopolymer or copolymer resins, and combinations thereof have a low air permeability coefficient.
[0004] JP-T-2018-536044 A JP-A-2018-193567 A
[0005] However, the rubber compositions described in Patent Documents 1 and 2 have room for improvement in the balance between gripping properties and breaking strength.
[0006] Therefore, the present inventors have conducted extensive research to solve the above problems and have surprisingly found that a tire manufactured using a polymer composition containing a specific rubber component and a specific raw material polymer has high grip performance and high breaking strength. Based on this finding, the present inventors have completed the present invention.
[0007] That is, the present invention provides the following: [1] A polymer composition comprising: a rubber component containing a conjugated diene polymer (A-1); and a raw material component polymer of a C9 fraction containing an aromatic olefin, wherein the conjugated diene polymer (A-1) contains structural units derived from a conjugated diene compound and structural units derived from an aromatic vinyl compound, the content of the structural units derived from the aromatic vinyl compound being 5% by mass or more and 60% by mass or less based on the total amount of the structural units derived from the conjugated diene compound and the structural units derived from the aromatic vinyl compound, and the content of the structural units derived from the aromatic vinyl compound is less than 40% by mass of aromatic vinyl compound single chains in which aromatic vinyl compounds are not consecutive, and the content of aromatic vinyl compound long chains in which 8 or more aromatic vinyl compound units are linked together is 10% by mass or less based on the content of the structural units derived from the aromatic vinyl compound. [2] The polymer composition according to [1], wherein the C9 fraction containing an aromatic olefin contains at least one selected from the group consisting of vinyltoluene, α-methylstyrene, styrene, indene, and methylindene. [3] The polymer composition according to [1] or [2], wherein the amount of protons per molecule of the raw material component polymer satisfies the following conditions: 0<amount of aromatic protons≦100 0≦amount of olefinic protons≦45. [4] The polymer composition according to any one of [1] to [3], wherein the number average molecular weight (Mn) of the raw material component polymer is 300 g / mol or more and less than 3000 g / mol. [5] The polymer composition according to any one of [1] to [4], wherein the content of the conjugated diene polymer (A-1) is 5 mass% or more of the total amount of the rubber component. [6] The polymer composition according to any one of [1] to [5], wherein the conjugated diene polymer (A-1) has a nitrogen-containing group and a hydrocarbyloxysilyl group. [7] The polymer composition according to any one of [1] to [6], further comprising a filler. [8] A rubber product formed using the polymer composition according to any one of [1] to [7]. [9] The rubber product according to [8], wherein the rubber product is selected from the group consisting of a tire, a tire tread, and a sidewall.
[0008] According to the present invention, a polymer composition capable of producing a tire product having high grip performance and high breaking strength can be provided. Furthermore, according to the present invention, a tire having high grip performance and high breaking strength can be produced.
[0009] In this specification, a range of values expressed as "A to B" is interpreted as including the value A as the lower limit and the value B as the upper limit.
[0010] [Polymer Composition] The polymer composition of the present invention contains a rubber component and a raw material polymer, and may further contain a filler and a silane coupling agent. A tire manufactured using the polymer composition of the present invention has high grip performance and high breaking strength. Each component contained in the polymer composition will be described in detail below. In this specification, the "rubber component" contained in the polymer composition refers to a polymer that can be thermally cured to give a cured product exhibiting rubber elasticity. The cured product exhibits the property of undergoing large deformation under small force at room temperature (for example, deformation that stretches to more than twice its original size when stretched at room temperature), and rapidly returning to almost its original shape when the force is removed.
[0011] (Rubber Component) The rubber component used in the polymer composition contains at least the conjugated diene polymer (A-1), and may further contain other rubber components other than A-1 (hereinafter simply referred to as "other rubber components").
[0012] (Conjugated Diene Polymer (A-1)) The conjugated diene polymer (A-1) contains a structural unit derived from a conjugated diene compound and a structural unit derived from an aromatic vinyl compound, and satisfies the following conditions (1) and (2): When the conjugated diene polymer (A-1) satisfies the following conditions (1) and (2), a tire having high grip performance and high breaking strength can be produced.
[0013] (1) The content of structural units derived from aromatic vinyl compounds is 5% by mass or more and 60% by mass or less, based on the total amount of structural units derived from conjugated diene compounds and structural units derived from aromatic vinyl compounds. The content of structural units derived from aromatic vinyl compounds is preferably 55% by mass or less, more preferably 50% by mass or less, and also preferably 10% by mass or more, more preferably 15% by mass or more, based on the total amount of structural units derived from conjugated diene compounds and structural units derived from aromatic vinyl compounds. The content ratio of structural units derived from aromatic vinyl compounds in the polymer is 1 This is a value measured by H-NMR.
[0014] (2) The content of aromatic vinyl compound single chains, in which aromatic vinyl compounds are not consecutive, is less than 40% by mass, preferably 38% by mass or less, and may be 1% by mass or more, 5% by mass or more, 10% by mass or more, 15% by mass or more, or 20% by mass or more, relative to the content of structural units derived from aromatic vinyl compounds, and the content of aromatic vinyl compound long chains, in which 8 or more aromatic vinyl compound units are consecutive, is 10% by mass or less, preferably 5% by mass or less, and may be 0.1% by mass or more, 0.2% by mass or more, or 0.5% by mass or more. The aromatic vinyl compound chains were calculated by decomposing a conjugated diene polymer with ozone and analyzing it by gel permeation chromatography (Tanaka et al., Polymer, 22, 1721 (1981)).
[0015] The conjugated diene polymer (A-1) preferably has a nitrogen-containing group and a hydrocarbyloxysilyl group. The term "hydrocarbyloxysilyl group" refers to a group in which at least one hydrocarbyloxy group is bonded to a silicon atom, and is represented by the following formula (1): (In formula (1), R 1 and R 2 are each independently a hydrocarbyl group. i is an integer of 1 to 3. When i is 1, multiple R 2 When i is 2 or 3, multiple R1 are the same or different. "*" indicates a bond.)
[0016] Examples of the nitrogen-containing group include a primary amino group, a secondary amino group, a tertiary amino group, a protected primary amino group, a protected secondary amino group, an imino group, an imidazolyl group, an azasilolizyl group, and a silazane structure. A primary amino group, a protected primary amino group, and an imino group are preferred, and a primary amino group is more preferred. In addition, the hydrocarbyloxysilyl group is a group represented by the above formula (1) in which i is 3 and R 1 is a group represented by a linear or branched alkyl group having 1 to 6 carbon atoms, and among the groups represented by the above formula (1), i is 2, and R 1 and R 2 are each independently a linear or branched alkyl group having 1 to 6 carbon atoms, preferably a triethoxysilyl group or a diethoxymethylsilyl group, more preferably a triethoxysilyl group. When the conjugated diene polymer (A-1) has a nitrogen-containing group and a hydrocarbyloxysilyl group, it exhibits good gripping properties and high breaking strength.
[0017] When a nitrogen-containing group and a hydrocarbyloxysilyl group are introduced into the conjugated diene polymer (A-1), the nitrogen-containing group and the hydrocarbyloxysilyl group may be introduced separately or simultaneously. Specific methods for introducing the nitrogen-containing group and the hydrocarbyloxysilyl group will be described in detail in the sections <Polymerization step> to <Modification step>.
[0018] The nitrogen-containing group and the hydrocarbyloxysilyl group may be introduced into the main chain terminal of the polymer, or into both the side chain and the main chain terminal of the polymer. Of these, it is preferable that the specific structure be introduced at least into the main chain terminal, in order to produce a tire with high grip performance and high breaking strength. Here, in this specification, the "main chain" of a polymer refers to the longest "trunk" portion of the atomic chain of the polymer. The "side chain" of a polymer refers to the portion branched from the "trunk" of the polymer.
[0019] The content of the conjugated diene polymer (A-1) is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 20% by mass or more, based on the total amount of the rubber component, and may be 100% by mass or less, 90% by mass or less, or 80% by mass or less. When the content of the conjugated diene polymer (A-1) is within the above range, a tire having high grip performance and high breaking strength can be produced.
[0020] (Method for Producing Conjugated Diene Polymer (A-1)) The conjugated diene polymer (A-1) can be obtained by copolymerizing a conjugated diene compound with an aromatic vinyl compound. Furthermore, a nitrogen-containing group and a hydrocarbyloxysilyl group can be introduced into the conjugated diene polymer (A-1) by reacting the conjugated diene polymer (A-1) with a compound having a nitrogen-containing group and a compound having a hydrocarbyloxysilyl group, or by reacting the conjugated diene polymer (A-1) with a compound having a nitrogen-containing group and a hydrocarbyloxysilyl group. These reactions are not particularly limited, but for example, the conjugated diene polymer (A-1) is preferably produced by a method including the following polymerization step. Matters related to the aspects of the present disclosure will be described in detail below.
[0021] <Polymerization Step> This step is a step of polymerizing a monomer containing a conjugated diene compound and an aromatic vinyl compound to obtain a conjugated diene polymer having an active terminal. Examples of conjugated diene compounds used in the polymerization include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, and 1,3-pentadiene. These conjugated diene compounds can be used alone or in combination of two or more.
[0022] The content of the structural units derived from the conjugated diene compound can be appropriately adjusted depending on the above condition (1) (the content of the structural units derived from the aromatic vinyl compound). The amount of the conjugated diene compound used is preferably 40% by mass or more and 95% by mass or less, more preferably 45% by mass or more and 95% by mass or less, and more preferably 50% by mass or more and 95% by mass or less, based on the total amount of the conjugated diene compound and the aromatic vinyl compound used in the polymerization.
[0023] Examples of aromatic vinyl compounds used in the polymerization include styrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, α-methylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 4-tert-butylstyrene, divinylbenzene, tert-butoxystyrene, vinylbenzyldimethylamine, (4-vinylbenzyl)dimethylaminoethyl ether, N,N-dimethylaminoethylstyrene, and vinylpyridine. These aromatic vinyl compounds can be used alone or in combination of two or more.
[0024] In the polymerization, a compound other than a conjugated diene compound and an aromatic vinyl compound (hereinafter also referred to as a "third monomer") may be used as a monomer. Examples of the third monomer other than a conjugated diene compound and an aromatic vinyl compound include acrylonitrile, methyl methacrylate, ethyl methacrylate, methyl acrylate, ethyl acrylate, hydroxyethyl methacrylate, and hydroxyethyl acrylate. These third monomers may be used alone or in combination of two or more.
[0025] The amount of the third monomer used is preferably 25% by mass or less, more preferably 15% by mass or less, and may be 0% by mass or more, based on the total amount of the monomers used in the polymerization.
[0026] The polymerization method used may be any of solution polymerization, gas phase polymerization, and bulk polymerization, with solution polymerization being particularly preferred. Furthermore, the polymerization format may be any of batch and continuous, with batch being preferred. When using solution polymerization, a specific example of the polymerization method is a method in which a monomer containing a conjugated diene compound and an aromatic vinyl compound is polymerized in an organic solvent in the presence of a polymerization initiator and, if necessary, a randomizer.
[0027] As the polymerization initiator, an alkali metal compound is used. Specific examples of the alkali metal compound include alkyllithiums such as methyllithium, ethyllithium, n-propyllithium, n-butyllithium, sec-butyllithium, and t-butyllithium; 1,4-dilithiobutane, phenyllithium, stilbenelithium, naphthyllithium, 1,3-bis(1-lithio-1,3-dimethylpentyl)benzene, 1,3-phenylenebis(3-methyl-1-phenylpentylidene)dilithium, naphthylsodium, naphthylpotassium, and ethoxypotassium. Among these, lithium compounds are preferred.
[0028] In the polymerization, a compound having a functional group that interacts with silica (hereinafter also referred to as an "initiating modifier") may be used as the alkali metal compound. By carrying out the polymerization in the presence of the initiating modifier, a functional group that interacts with silica can be introduced into the polymerization initiation terminal of the conjugated diene polymer (A-1). In this specification, "a functional group that interacts with silica" means a group having an element that interacts with silica, such as nitrogen, sulfur, phosphorus, or oxygen. "Interaction" means forming a covalent bond between molecules or forming an intermolecular force that is weaker than a covalent bond (for example, an electromagnetic force acting between molecules such as an ion-dipole interaction, a dipole-dipole interaction, a hydrogen bond, or a van der Waals force).
[0029] The initiating modifier is preferably a nitrogen-containing alkali metal compound, particularly a mixture of a non-nitrogen-containing alkali metal compound and a secondary amine compound. In the mixture, examples of the secondary amine compound include linear or cyclic secondary amine compounds such as dimethylamine, diethylamine, dipropylamine, dibutylamine, dodecamethyleneimine, N,N'-dimethyl-N'-trimethylsilyl-1,6-diaminohexane, piperidine, pyrrolidine, hexamethyleneimine, heptamethyleneimine, dicyclohexylamine, N-methylbenzylamine, di-(2-ethylhexyl)amine, diallylamine, morpholine, N-(trimethylsilyl)piperazine, N-(tert-butyldimethylsilyl)piperazine, 1,3-ditrimethylsilyl-1,3,5-triazinane, N-trimethylsilylpiperazine, 1,3,3-trimethyl-6-azabicyclo[3.2.1]octane, and 1-propyl-3-azabicyclo[3.2.2]nonane. As the nitrogen-free alkali metal compound, it is preferable to use an alkyllithium.
[0030] When polymerization is carried out in the presence of the above mixture, the nitrogen-free alkali metal compound and the secondary amine compound may be mixed in advance, and the mixture may be added to the polymerization system to carry out polymerization. Alternatively, the nitrogen-free alkali metal compound and the secondary amine compound may be added to the polymerization system, and the two may be mixed in the polymerization system to carry out polymerization. By carrying out polymerization in the presence of a mixture of the nitrogen-free alkali metal compound and the secondary amine compound, a nitrogen-containing group can be introduced into the main chain terminal of the conjugated diene polymer (A-1).
[0031] The amount of polymerization initiator used (the total amount when two or more types are used) is preferably 0.01 to 20 mmol, more preferably 0.05 to 15 mmol, per 100 g of monomer used in the synthesis of the conjugated diene polymer (A-1). The proportion of initiator modifier used may be 10 mol % to 100 mol % based on the total amount of polymerization initiator (preferably alkali metal compound) used in the polymerization of the monomer.
[0032] Randomizers can be used for purposes such as adjusting the vinyl bond content, which indicates the content of vinyl bonds in a polymer, and adjusting the proportions of aromatic vinyl compound single chains and aromatic vinyl compound long chains. Examples of randomizers include dimethoxybenzene, tetrahydrofuran, dimethoxyethane, diethylene glycol dibutyl ether, diethylene glycol dimethyl ether, 2,2-di(tetrahydrofuryl)propane, 2-(2-ethoxyethoxy)-2-methylpropane, triethylamine, pyridine, N-methylmorpholine, and tetramethylethylenediamine; and at least one potassium salt selected from the group consisting of potassium alkoxides, potassium phenoxide, potassium salts of organic carboxylic acids, potassium salts of organic sulfonic acids, and potassium salts of organic phosphorous acid partial esters. The randomizers exemplified above can be used alone or in combination of two or more. Among these, potassium salts are preferred, and a combination of potassium salts and the randomizers other than potassium salts is more preferred.
[0033] The organic solvent used in the polymerization may be any organic solvent inert to the reaction, and examples thereof include aliphatic hydrocarbons, alicyclic hydrocarbons, and aromatic hydrocarbons. Among these, hydrocarbons having 3 to 8 carbon atoms are preferred, and specific examples thereof include propane, n-butane, isobutane, n-pentane, isopentane, n-hexane, cyclohexane, propene, 1-butene, isobutene, trans-2-butene, cis-2-butene, 1-pentyne, 2-pentyne, 1-hexene, 2-hexene, benzene, toluene, xylene, ethylbenzene, heptane, cyclopentane, methylcyclopentane, methylcyclohexane, 1-pentene, 2-pentene, and cyclohexene. These organic solvents may be used alone or in combination of two or more.
[0034] When solution polymerization is performed, the monomer concentration in the reaction solvent is preferably 5 to 50% by mass, more preferably 10 to 30% by mass, from the viewpoint of maintaining a balance between productivity and ease of polymerization control. The temperature of the polymerization reaction is preferably −20° C. to 150° C., more preferably 0 to 120° C. Furthermore, the polymerization reaction is preferably carried out under a pressure sufficient to maintain the monomer substantially in a liquid phase. Such a pressure can be obtained by, for example, pressurizing the inside of a reactor with a gas inert to the polymerization reaction.
[0035] By such a polymerization reaction, a conjugated diene polymer having an active terminal can be obtained. The weight average molecular weight (Mw) of the obtained conjugated diene polymer, measured by gel permeation chromatography (GPC) in terms of polystyrene, is preferably 5.0×10 4 ~1.0 x 10 6 Mw is 5.0 × 10 4 If it is smaller than 1.0 × 10, the tensile strength, low heat buildup and abrasion resistance of the crosslinked polymer tend to be easily reduced. 6 If it is larger than 8.0 × 10, the processability of the polymer composition obtained using the conjugated diene polymer tends to be easily reduced. 4 ~9.0 x 10 6 and more preferably 1.0 × 10 5 ~8.0 x 10 5 is.
[0036] In a conjugated diene polymer having an active terminal, the vinyl bond content in the butadiene unit (hereinafter also referred to as "vinyl content") is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more. The vinyl content is preferably 70% by mass or less, more preferably 68% by mass or less, and even more preferably 65% by mass or less. When the vinyl content is 10% by mass or more, the grip properties tend to be improved, and when it is 70% by mass or less, the abrasion resistance of the obtained vulcanized rubber tends to be improved. In this specification, "vinyl content" is a value indicating the content ratio of structural units having 1,2-bonds to all structural units of butadiene in the conjugated diene polymer, 1 This is a value measured by H-NMR.
[0037] <Modification Step> The method for producing the conjugated diene polymer (A-1) may include a modification step in addition to the polymerization step. In this step, an active terminal of the conjugated diene polymer obtained in the polymerization step is reacted with a compound having a hydrocarbyloxysilyl group. This reaction allows a conjugated diene polymer having a hydrocarbyloxysilyl group to be obtained. In this specification, the term "active terminal" refers to a portion (more specifically, a carbon anion) that is present at the end of a molecular chain and that constitutes a carbon-metal bond.
[0038] The compound having a hydrocarbyloxysilyl group is preferably a compound having both a nitrogen-containing group and a hydrocarbyloxysilyl group in one molecule (hereinafter also referred to as a "terminal modifier"). Examples of the terminal modifier that can be used include an amino group-containing alkoxysilane compound, an imino group-containing alkoxysilane compound, an imidazolyl group-containing alkoxysilane compound, and an alkoxysilane compound having an azasilolidine structure. Examples of amino group-containing alkoxysilane compounds include N,N-bis(trimethylsilyl)aminopropylmethyldimethoxysilane, N,N-bis(trimethylsilyl)aminopropyltrimethoxysilane, N,N-bis(trimethylsilyl)aminopropyltriethoxysilane, N,N-bis(trimethylsilyl)aminopropylmethyldiethoxysilane, N,N-bis(trimethylsilyl)aminoethyltrimethoxysilane, N,N-bis(trimethylsilyl)aminoethyltriethoxysilane, N,N-bis(trimethylsilyl)aminoethylmethyldimethoxysilane, and N,N-bis(trimethylsilyl)aminoethylmethyldiethoxysilane.
[0039] Other examples of amino group-containing alkoxysilane compounds include tris(2-triethoxysilylethyl)amine, tris(3-triethoxysilylpropyl)amine, tris(5-triethoxysilylpentyl)amine, N,N,N',N'-tetra(2-triethoxysilylethyl)-1,2-diaminoethane, N,N,N',N'-tetra(3-triethoxysilylpropyl)-1,3-diaminopropane, and N,N,N-tris(triethoxysilyl)propylamine, as well as compounds in which the alkyl groups and alkanediyl groups in these compounds are replaced with alkyl groups having 1 to 6 carbon atoms and alkanediyl groups having 1 to 6 carbon atoms, respectively.
[0040] Other examples of imino group-containing alkoxysilanes include N-(1,3-dimethylbutylidene)-3-(triethoxysilyl)-1-propanamine, N-(1-methylpropylidene)-3-(triethoxysilyl)-1-propanamine, N-(4-N,N-dimethylaminobenzylidene)-3-(triethoxysilyl)-1-propanamine, N-(cyclohexylidene)-3-(triethoxysilyl)-1-propanamine, and trimethoxysilyl compounds, methyldiethoxysilyl compounds, ethyldimethoxysilyl compounds, 3-hexamethyleneiminopropyltrimethoxysilane, and 3-hexamethyleneiminopropylmethyldimethoxysilane corresponding to these triethoxysilyl compounds, as well as compounds in which the alkyl groups and alkylene groups in the above compounds are replaced with alkyl groups and alkylene groups having 1 to 6 carbon atoms.
[0041] Other examples of imidazolyl group-containing alkoxysilanes include N-(3-trimethoxysilylpropyl)-4,5-dihydroimidazole, N-(3-triethoxysilylpropyl)-4,5-dihydroimidazole, N-(3-trimethoxysilylpropyl)-4,5-imidazole, N-(3-triethoxysilylpropyl)-4,5-imidazole, and N,N-bis(triethoxysilylpropyl)aminopropyl-1-imidazole, as well as compounds in which the alkyl groups and alkanediyl groups in the above compounds are replaced with alkyl groups and alkanediyl groups having 1 to 6 carbon atoms.
[0042] Examples of alkoxysilane compounds having an azacilloridine structure include 1-trimethylsilyl-2,2-dimethoxy-1-aza-2-silacyclopentane, 1-triethylsilyl-2,2-diethoxy-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(3-trimethoxysilylpropyl)-1,2-azasilolidine, 2,2-dimethoxy-1-phenyl-1,2-azasilolidine, and 2-(2,2-dimethoxy-1,2-azasilolidine-1-yl)-N,N-diethylethan-1-amine.
[0043] As the terminal modifying agent, one of these may be used alone, or two or more may be used in combination.
[0044] The reaction between the polymerization active terminal and the terminal-modifying agent is preferably carried out as a solution reaction. This solution reaction may be carried out using a solution containing unreacted monomers after the polymerization reaction is completed, or may be carried out after isolating the conjugated diene polymer contained in the solution and dissolving it in a suitable solvent such as cyclohexane. The reaction may be carried out either batchwise or continuously. In this case, the method of adding the terminal-modifying agent is not particularly limited, and examples thereof include a method of adding it all at once, a method of adding it in portions, and a method of adding it continuously.
[0045] The amount of the terminal modifier used in the above reaction may be appropriately determined depending on the type of compound used in the reaction, but is preferably 0.1 molar equivalents or more, more preferably 0.3 molar equivalents or more, relative to the metal atoms involved in the polymerization reaction of the polymerization initiator. By using an amount of terminal modifier of 0.1 molar equivalents or more in the above reaction, the modification reaction can be sufficiently promoted, and the dispersibility of the filler can be suitably improved. Furthermore, in order to avoid the addition of an excessive amount of terminal modifier, the amount of terminal modifier used is preferably 1.5 molar equivalents or less, more preferably 1.2 moles or less, relative to the metal atoms involved in the polymerization reaction of the polymerization initiator.
[0046] The reaction temperature is usually the same as the polymerization reaction temperature, and is preferably -20°C to 150°C, and more preferably 0 to 120°C. If the reaction temperature is too low, the viscosity of the modified conjugated diene polymer tends to increase. On the other hand, if the reaction temperature is too high, the active polymerization terminals are likely to be deactivated. The reaction time is preferably 1 minute to 5 hours, and more preferably 2 minutes to 1 hour.
[0047] In addition, when producing a conjugated diene polymer, a treatment of reacting the polymerization active terminal with a coupling agent may be carried out for the purpose of increasing the Mooney viscosity and cold flow characteristics of the polymer. Hereinafter, the reaction between the polymerization active terminal and the coupling agent will also be referred to as a "coupling reaction." The reaction using the coupling agent may be carried out before or after the reaction between the polymerization active terminal and the terminal-terminating end-modifying agent, or may be carried out simultaneously with the reaction between the polymerization active terminal and the terminal-terminating end-modifying agent. Alternatively, the coupling agent alone may be used without using the terminal-terminating end-modifying agent. Specific examples of coupling agents include 2,4-tolylene diisocyanate, diphenylmethane diisocyanate, N,N,N',N'-tetramethylphthalamide, tetrachlorosilicon, N,N,N',N'-tetramethyl-4,4'-diaminobenzophenone, and tin tetrachloro.
[0048] Furthermore, when a compound having a protecting group (such as a trimethylsilyl group) is used as the terminal modifier, a conjugated diene polymer having a protecting group derived from the terminal modifier may be partially or completely substituted with hydrogen to obtain a polymer, which may be used as the conjugated diene polymer in the subsequent steps. Furthermore, when a protecting group-containing compound is used as the terminal modifier, the conjugated diene polymer modified with the terminal modifier may be further reacted with an onium salt generator. In this case, a polymer having an onium salt structure at the polymer terminal can be obtained as the conjugated diene polymer. Having an onium salt structure in the conjugated diene polymer is preferred in that it can improve the shape retention of a crosslinked body obtained using the polymer composition.
[0049] The conjugated diene polymer contained in the reaction solution can be isolated by a known solvent removal method such as steam stripping and a drying procedure such as heat treatment. The weight average molecular weight (Mw) of the conjugated diene polymer measured by gel permeation chromatography (GPC) in terms of polystyrene is preferably 1.0 × 10 5 or more. Mw is 1.0 × 10 5 If the Mw of the conjugated diene polymer is smaller than 1.2×10, the crosslinked product tends to have reduced shape stability, tensile strength, and abrasion resistance.5 More preferably, 1.5 × 10 5 The Mw of the conjugated diene polymer is preferably 1.5×10 6 Mw is 1.5 × 10 or less. 6 If the Mw of the conjugated diene polymer is larger than 1.3×10, the processability of the polymer composition tends to be easily reduced. 6 More preferably, 1.0 × 10 6 The following is the result.
[0050] As described above, a conjugated diene polymer A-1 can be obtained by a method including a <polymerization step>. Furthermore, by using an initiating modifier in the <polymerization step>, a conjugated diene polymer A-1 having a nitrogen-containing group can be obtained. Furthermore, by passing through a <modification step>, a conjugated diene polymer A-1 having a nitrogen-containing group and a hydrocarbyloxysilyl group can be obtained.
[0051] (Other Rubber Components) The other rubber components are not particularly limited as long as they do not satisfy the conditions for the conjugated diene polymer (A-1). Examples of the other rubber components include butadiene rubber (BR, for example, high-cis BR having 90% or more cis-1,4 bonds), emulsion-polymerized or solution-polymerized styrene-butadiene rubber (SBR), styrene-isoprene-butadiene rubber, styrene-isoprene rubber, partially hydrogenated styrene-butadiene rubber, styrene-α-methylstyrene-butadiene rubber, ethylene-propylene-diene rubber, natural rubber (NR), isoprene rubber (IR), isoprene-butadiene rubber, and halogenated isoprene rubber, liquid rubber, ethylene-propylene rubber (EPM), ethylene-propylene-diene rubber (EPDM), and silicone rubber.
[0052] Examples of liquid rubbers include liquid polyisoprene (liquid IR), liquid polybutadiene (liquid BR), liquid styrene-butadiene copolymer (liquid SBR), and liquid ethylene-propylene copolymer (liquid EP). For example, liquid SBR having a weight-average molecular weight of 1,000 to 100,000, preferably 2,000 to 80,000, can be used. The weight-average molecular weight here refers to the weight-average molecular weight in terms of polystyrene as analyzed by gel permeation chromatography (GPC). The liquid rubber used in this disclosure refers to one that has fluidity at 23°C.
[0053] The content of the other rubber component can be appropriately adjusted depending on the content of the conjugated diene polymer (A-1). For example, the content of the other rubber component is preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 85% by mass or less, based on the total amount of the rubber component, and may also be 0% by mass, 5% by mass or more, or 10% by mass or more.
[0054] The content of the rubber component is preferably 20% by mass or more and 70% by mass or less, more preferably 25% by mass or more and 65% by mass or less, and even more preferably 30% by mass or more and 60% by mass or less, based on the total amount of the polymer composition. When the content of the rubber component is within the above range, a tire having high grip performance and high breaking strength can be produced.
[0055] (Raw material polymer) The raw material polymer used in the polymer composition is a raw material polymer of a C9 fraction containing an aromatic olefin. In the present invention, the "raw material polymer" refers to a polymer obtained by polymerizing a raw material (a C9 fraction containing an aromatic olefin). By using such a raw material polymer, a tire having high grip performance and high breaking strength can be manufactured.
[0056] The C9 fraction containing aromatic olefins is generally a fraction obtained by thermal cracking of petroleum (such as naphtha), which has a boiling point range of about 100 to 280°C and mainly contains compounds having 8 to 10 carbon atoms. Examples of aromatic olefins in the C9 fraction include vinyltoluene, α-methylstyrene, styrene, indene, and methylindene, and two or more of these may be contained.
[0057] The feedstock components may further contain components other than the C9 fraction containing aromatic olefins. Examples of the other components include non-polymerizable hydrocarbons that do not have polymerizable groups and do not participate in polymerization. Examples of non-polymerizable hydrocarbons include saturated hydrocarbons (e.g., alkanes, cycloalkanes), and aromatic hydrocarbons (e.g., benzene, methylethylbenzene, toluene).
[0058] The polymerization method of the raw material components is not particularly limited, and can be carried out by a conventionally known method. Examples of the polymerization method include thermal polymerization and cationic polymerization, with thermal polymerization being preferred. The reaction temperature of the thermal polymerization is not particularly limited, and is, for example, preferably 250°C or higher and 300°C or lower, and more preferably 260°C or higher and 290°C or lower. The reaction time of the thermal polymerization is not particularly limited, and is, for example, preferably 1 hour or higher and 10 hours or lower, more preferably 2 hours or higher and 7 hours or lower, and even more preferably 3 hours or higher and 5 hours or lower.
[0059] The number average molecular weight (Mn) of the raw material component polymer is not particularly limited, but is, for example, preferably 300 g / mol or more but less than 3000 g / mol, more preferably 400 g / mol or more, even more preferably 450 g / mol or more, even more preferably 500 g / mol or more, even more preferably 550 g / mol or more, and more preferably 2500 g / mol or less, even more preferably 2000 g / mol or less, even more preferably 1500 g / mol or less, particularly preferably 1300 g / mol or less, and most preferably 1100 g / mol or less. If the number average molecular weight (Mn) of the raw material component polymer is within the above numerical range, compatibility with the rubber component will be improved, and the viscoelastic properties, which are an indicator of high grip performance, will be improved. The number average molecular weight (Mn) of the raw material component polymer can be measured by a conventionally known GPC (gel permeation chromatography) analysis method. In the present invention, the value is measured by the method described in the Examples below.
[0060] The proton amount per molecule of the raw material component polymer preferably satisfies the following conditions: 0<aromatic proton amount≦100 0≦olefin proton amount≦45, more preferably satisfies 0<aromatic proton amount≦80 0≦olefin proton amount≦20, further preferably satisfies 0<aromatic proton amount≦60 0≦olefin proton amount≦10, and particularly preferably satisfies 0<aromatic proton amount≦40 0≦olefin proton amount≦5. If the proton amount per molecule of the raw material component polymer satisfies the above conditions, compatibility with the rubber component will be improved, and the viscoelastic properties, which are an index of high grip performance, will be improved. The proton amount per molecule of the raw material component polymer can be determined by the conventionally known 1 In the present invention, the value is measured by the method described in the Examples below.
[0061] The raw material polymer may be hydrogenated. The method for hydrogenating the raw material polymer is not particularly limited and can be carried out by a conventionally known method. The hydrogenation method can be carried out, for example, by contacting the raw material polymer with a hydrogenation catalyst in the presence of molecular hydrogen. The hydrogenation catalyst is not particularly limited and examples thereof include nickel-based catalysts, molybdenum-based catalysts, cobalt-based catalysts, palladium-based catalysts, and platinum-based catalysts. The hydrogenation reaction temperature is not particularly limited and is, for example, preferably 150°C to 320°C, more preferably 160°C to 300°C. The hydrogenation reaction pressure is not particularly limited and is, for example, preferably 2 MPa to 30 MPa, more preferably 3 MPa to 25 MPa. The hydrogenation reaction time is not particularly limited and is, for example, preferably 1 hour to 10 hours, more preferably 2 hours to 7 hours, and even more preferably 3 hours to 5 hours.
[0062] (Other Resins) The polymer composition may further contain other resins in addition to the raw material component polymers. Examples of other resins include rosin-based resins, terpene-based resins, coumarone-based resins, and phenol-based resins.
[0063] (Filler) Examples of fillers include silica, carbon black, and inorganic compounds represented by the following formula (2) (hereinafter also referred to as "inorganic compound (M)"), reinforcing fibers (for example, inorganic fibers such as glass fiber and carbon fiber, and organic fibers such as nylon and polyester), and barium sulfate. Among these, it is preferable to use at least one selected from the group consisting of silica, carbon black, and inorganic compound (M). nM 1 mSiO k ・iH 2 O...(2) (In formula (2), M 1 is at least one selected from the group consisting of a specific metal, which is any one of aluminum, magnesium, titanium, and calcium, an oxide of the specific metal, a hydroxide of the specific metal, a hydrate of an oxide of the specific metal, and a hydrate of a hydroxide of the specific metal. n is an integer of 1 to 5, m is an integer of 0 to 10, k is an integer of 2 to 5, and i is an integer of 0 to 10.
[0064] (Silica) The silica is not particularly limited, but examples thereof include dry process silica, wet process silica, colloidal silica, and precipitated silica. Among these, wet process silica containing hydrous silicic acid as the main component is preferred. These silicas can be used alone or in combination of two or more. The BET specific surface area of the silica (measured in accordance with ISO 5794 / 1) is 40 to 350 m 2 / g, and 80 to 300m 2 / g is more preferably in the range of 120 to 250m 2 / g is particularly preferred. Silica having a BET specific surface area in this range has the advantage of being able to achieve both rubber reinforcing properties and dispersibility in the conjugated diene polymer (A-1). Examples of such silica include "Nipsil AQ" (BET specific surface area = 205 m), manufactured by Tosoh Silica Corporation. 2 / g), "Nipsil KQ", product name "Ultrasil VN3" (BET specific surface area = 175 m), manufactured by Degussa 2 Commercially available products such as PEG-100 / g can be used.
[0065] The silica contained in the polymer composition may be a mixture of two or more types having different specific surface areas. Specifically, CTAB (cetyltrimethylammonium bromide) having a specific surface area of 180 m 2 / g or more, BET specific surface area is 185m 2 / g or more and an aggregate size of 45 nm or more; and a first silica having a CTAB specific surface area of 95 m 2 / g or less, BET specific surface area is 100m 2 The CTAB specific surface area of the silica is measured in accordance with ASTM D3765-92.
[0066] The polymer composition has a CTAB specific surface area of 180 m 2 / g or more, BET specific surface area is 185m 2 / g or more and an aggregate size of 45 nm or more; and a first silica having a CTAB specific surface area of 95 m 2 / g or less, BET specific surface area is 100m 2 / g or less of a second silica. By using such a first silica and a second silica in combination, it becomes possible to satisfactorily disperse the first silica, which has a small average primary particle size but a relatively large aggregate size, in the rubber component. This improves the dispersibility of the silica, and provides excellent rubber breaking strength, abrasion resistance, fuel economy, and processability.
[0067] The CTAB specific surface area of the first silica is preferably 190 m 2 / g or more, more preferably 195m 2 / g or more, more preferably 197m 2 / g or more. CTAB specific surface area is 190 m 2 When the CTAB specific surface area of the first silica is 350 m / g or more, sufficient improvement in rubber breaking strength and abrasion resistance tends to be easily obtained. 2 / g or less, more preferably 300m 2 / g or less, more preferably 250m 2 / g or less. CTAB specific surface area is 350 m 2 When the molecular weight is 1 / g or less, the particles have excellent dispersibility and are less likely to aggregate, and therefore tend to easily maintain their physical properties.
[0068] The BET specific surface area of the first silica is preferably 190 m 2 / g or more, more preferably 195m 2 / g or more, more preferably 210m 2 / g or more. BET specific surface area is 190 m 2 When the BET specific surface area of the first silica is 350 m / g or more, sufficient improvement in rubber breaking strength and abrasion resistance tends to be easily obtained. 2 / g or less, more preferably 300m 2 / g or less, more preferably 260m 2 / g or less. BET specific surface area is 350 m 2 When the BET specific surface area of silica is 1 / g or less, the silica has excellent dispersibility and is less likely to aggregate, so that the physical properties tend to be easily maintained. The BET specific surface area of silica is measured in accordance with ASTM D3037-81.
[0069] The aggregate size of the first silica is 45 nm or more, preferably 50 nm or more, more preferably 55 nm or more, and even more preferably 60 nm or more. The aggregate size of the first silica is preferably 100 nm or less, more preferably 80 nm or less, even more preferably 70 nm or less, and particularly preferably 67 nm or less. By having such an aggregate size, it is possible to provide excellent fuel economy and abrasion resistance while maintaining good dispersibility (processability). The aggregate size of silica can be measured by the method described in JP 2011-140613 A.
[0070] The average primary particle diameter of the first silica is preferably 25 nm or less, more preferably 22 nm or less, even more preferably 17 nm or less, and particularly preferably 14 nm or less. The lower limit of the average primary particle diameter of the first silica is not particularly limited, but is preferably 3 nm or more, more preferably 5 nm or more, and even more preferably 7 nm or more. Although it has such a small average primary particle diameter, the carbon black-like structure having the above aggregate size can further improve the dispersibility (processability) of the silica, thereby further improving fuel economy and wear resistance. The average primary particle diameter of the silica can be determined by observing the silica with a transmission or scanning electron microscope, measuring the particle diameters of 400 or more primary silica particles observed in the field of view, and averaging the measured values.
[0071] The CTAB specific surface area of the second silica is preferably 10 m 2 / g or more, more preferably 20m 2 / g or more, more preferably 30m 2 / g or more. 2 When the CTAB specific surface area of the second silica is 80 m / g or more, the reinforcing property is high, and it is easy to ensure the mechanical strength and abrasion resistance required for the polymer composition used in the production of tires. 2 / g or less, more preferably 60m 2 / g or less, more preferably 50m 2 / g or less. CTAB specific surface area is 80 m 2 When the silica content is 1 / g or less, the dispersibility of the silica is improved, and the rubber breaking strength and abrasion resistance are easily improved.
[0072] The BET specific surface area of the second silica is preferably 10 m 2 / g or more, more preferably 20m 2 / g or more, more preferably 30m 2 / g or more. BET specific surface area is 10 m 2 When the BET specific surface area of the second silica is 85 m / g or more, the reinforcing property is high, and it is easy to ensure the mechanical strength and abrasion resistance required for the polymer composition used in manufacturing a tire. 2 / g or less, more preferably 60m 2 / g or less, more preferably 50m 2 / g or less. BET specific surface area is 85 m 2 When the silica content is 1 / g or less, the dispersibility of the silica is improved, and the rubber breaking strength and abrasion resistance are easily improved.
[0073] The average primary particle size of the second silica is preferably 20 nm or more, more preferably 25 nm or more, even more preferably 30 nm or more, particularly preferably 35 nm or more, and most preferably 55 nm or more.The upper limit of the average primary particle size of the second silica is not particularly limited, but is preferably 500 nm or less, more preferably 200 nm or less, even more preferably 100 nm or less, particularly preferably 70 nm or less.By having such an average primary particle size, rubber breaking strength and abrasion resistance can be improved.
[0074] (Carbon Black) The carbon black is not particularly limited, and examples thereof include GPF, FEF, HAF, ISAF, and SAF grade carbon black. The nitrogen adsorption specific surface area (N 2 SA) is not particularly limited, but is preferably 50 to 200 m because the effects of the present disclosure are more excellent. 2 / g is preferred, and 70 to 150m 2 / g is more preferable. 2The specific surface area (SA) is the amount of nitrogen adsorption on the surface of the carbon black measured in accordance with JIS K6217-2:2001 "Part 2: Determination of specific surface area - Nitrogen adsorption method - Single point method." Carbon black may be used alone or in combination of two or more types. The amount of carbon black mixed is preferably in the range of 1 to 150 parts by mass, more preferably 5 to 120 parts by mass, per 100 parts by mass of the rubber component.
[0075] (Inorganic Filler) Specific examples of the inorganic compound (M) include compounds in which the specific metal is aluminum, such as aluminum oxide, alumina monohydrate, aluminum hydroxide, aluminum carbonate, aluminum silicate, and calcium aluminum oxide (Al 2 O 3 CaO 2SiO 4 and the like); compounds in which the specific metal is magnesium include, for example, magnesium oxide, magnesium hydroxide, magnesium carbonate, magnesium silicate, and calcium magnesium silicate (CaMgSiO 4 ), talc, etc.; compounds in which the specific metal is titanium include, for example, titanium oxide, etc.; and compounds in which the specific metal is calcium include, for example, calcium oxide, calcium hydroxide, calcium carbonate, calcium silicate, etc.
[0076] The total amount of the filler is preferably 10 parts by mass or more and 200 parts by mass or less, more preferably 30 parts by mass or more and 150 parts by mass or less, and even more preferably 50 parts by mass or more and 120 parts by mass or less, based on 100 parts by mass of the rubber component.
[0077] (Silane Coupling Agent) When silica is blended, it is preferable to blend a silane coupling agent. Known silane coupling agents can be used as the silane coupling agent. Examples include bis[3-(triethoxysilyl)propyl]tetrasulfide, bis[3-(triethoxysilyl)propyl]disulfide, 3-[ethoxybis(3,6,9,12,15-pentaoxaoctacosan-1-yloxy)silyl]-1-propanethiol, 3-mercaptopropyltrimethoxysilane, 3-octanoylthio-1-propyltriethoxysilane), and their homocondensates or cocondensates with 3-mercaptopropyltriethoxysilane. Commercially available bis[3-(triethoxysilyl)propyl]tetrasulfides may be used, such as Si-69 manufactured by Evonik. Commercially available bis[3-(triethoxysilyl)propyl]disulfide may also be used, such as Si-75 manufactured by Evonik. Commercially available 3-[ethoxybis(3,6,9,12,15-pentaoxaoctacosan-1-yloxy)silyl]-1-propanethiol may also be used, such as Si-363 manufactured by Evonik. Commercially available 3-mercaptopropyltrimethoxysilane may also be used, such as KBM803 manufactured by Shin-Etsu Chemical Co., Ltd. Commercially available 3-octanoylthio-1-propyltriethoxysilane may also be used, such as NXT-Silane manufactured by Momentive. Commercially available condensates of 3-octanoylthio-1-propyltriethoxysilane may also be used, such as NXT-Z45 silane manufactured by Momentive. These silane coupling agents can be used alone or in combination of two or more. The content of the silane coupling agent is preferably 1 part by mass or more and 30 parts by mass or less, and more preferably 2 parts by mass or more and 20 parts by mass or less, per 100 parts by mass of silica.
[0078] (Other Additives) The polymer composition of the present invention may contain other additives such as a vulcanizing agent, a vulcanization accelerator, a vulcanization acceleration aid, an antioxidant, a softener, an antioxidant, and a colorant, within a range that does not impair the functions of the polymer composition.
[0079] Examples of the vulcanizing agent include sulfur-based vulcanizing agents such as powdered sulfur, precipitated sulfur, highly dispersible sulfur, surface-treated sulfur, insoluble sulfur, dimorpholine disulfide, and alkylphenol disulfide, as well as zinc oxide, magnesium oxide, litharge, p-quinone dioxime, p-dibenzoylquinone dioxime, tetrachloro-p-benzoquinone, poly-p-dinitrobenzene, methylene dianiline, phenol resin, brominated alkylphenol resin, and chlorinated alkylphenol resin. The amount of the vulcanizing agent is preferably 0.1 part by mass or more and 10 parts by mass or less, and more preferably 1 part by mass or more and 5 parts by mass or less, per 100 parts by mass of the rubber component.
[0080] Examples of vulcanization accelerators include thiuram-based accelerators such as tetramethylthiuram disulfide (TMTD), tetraethylthiuram disulfide (TETD), and tetramethylthiuram monosulfide (TMTM), aldehyde-ammonia-based accelerators such as hexamethylenetetramine, guanidine-based accelerators such as diphenylguanidine (DPG), thiazole-based accelerators such as 2-mercaptobenzothiazole (MBT) and dibenzothiazyl disulfide (DM), sulfenamide-based accelerators such as N-cyclohexyl-2-benzothiazylsulfenamide (CBS) and N-t-butyl-2-benzothiazylsulfenamide (BBS), and dithiocarbamate-based accelerators such as zinc dimethyldithiocarbamate (ZnPDC). The amount of the vulcanization accelerator per 100 parts by mass of the rubber component is preferably 0.1 to 10 parts by mass, and more preferably 1 to 5 parts by mass.
[0081] Examples of the vulcanization accelerator aid include fatty acids, fatty acid zinc salts, zinc oxide, etc. As fatty acids, acetic acid, propionic acid, butanoic acid, stearic acid, acrylic acid, maleic acid, etc. can be used. As fatty acid zinc salts, zinc acetate, zinc propionate, zinc butyrate, zinc stearate, zinc acrylate, zinc maleate, etc. can be used. As fatty acid zinc salts, salts of the above fatty acid zinc salts can be used. The content of the vulcanization accelerator aid is preferably 0.1 parts by mass or more and 10 parts by mass or less, more preferably 1 part by mass or more and 5 parts by mass or less, per 100 parts by mass of the rubber component.
[0082] Examples of the antioxidant include aliphatic and aromatic hindered amine compounds, hindered phenol compounds, etc. The amount of the antioxidant is preferably 0.1 parts by mass or more and 10 parts by mass or less, and more preferably 1 part by mass or more and 5 parts by mass or less, per 100 parts by mass of the rubber component.
[0083] Examples of the antioxidant include butylhydroxytoluene (BHT), butylhydroxyanisole (BHA), etc. The amount of the antioxidant is preferably 0.1 part by mass or more and 10 parts by mass or less, and more preferably 1 part by mass or more and 5 parts by mass or less, per 100 parts by mass of the rubber component.
[0084] The softener may be any conventionally known softener, and is not particularly limited. Examples include petroleum-based softeners such as aromatic oil, paraffin oil, and naphthenic oil, and plant-based softeners such as palm oil, castor oil, cottonseed oil, and soybean oil. One or more of these may be used alone or in combination. When a softener is contained, from the viewpoint of ease of handling, it is preferable to contain a softener that is liquid at room temperature, such as 25°C, among the softeners described above, such as petroleum-based softeners, such as aromatic oil, paraffin oil, and naphthenic oil, with aromatic oil being particularly preferred. The content of the softener is preferably 10 parts by mass or more and 200 parts by mass or less, more preferably 20 parts by mass or more and 100 parts by mass or less, per 100 parts by mass of the rubber component.
[0085] Examples of the colorant include inorganic pigments such as titanium dioxide, zinc oxide, ultramarine, red iron oxide, lithopone, lead, cadmium, iron, cobalt, aluminum, hydrochlorides, sulfates, etc., azo pigments, copper phthalocyanine pigments, etc. The amount of the colorant per 100 parts by mass of the rubber component is preferably 0.1 part by mass to 10 parts by mass, more preferably 1 part by mass to 5 parts by mass.
[0086] The other additives can be kneaded with the rubber component in a known rubber kneading machine, such as a roll, a Banbury mixer, a kneader, etc., and vulcanized under any conditions to be used as a polymer composition. The amount of the other additives to be added can be any conventional amount as long as it does not contradict the object of the present invention.
[0087] [Method for producing polymer composition] The method for producing the polymer composition of the present invention comprises a step of kneading at least the rubber component and the raw material component polymer. Preferably, the method for producing the polymer composition may further comprise a step of kneading the vulcanizing agent. More preferably, the method may further comprise a step of kneading the vulcanizing agent and the vulcanization accelerator.
[0088] In the method for producing the polymer composition, the above-mentioned other additives may be appropriately blended and kneaded within the range that does not impair the function of the polymer composition.
[0089] For producing the polymer composition, a conventionally known kneading device can be used, and the kneading temperature, time, compounding order, etc. can be appropriately selected.
[0090] [Rubber Products] Using the polymer composition of the present invention, rubber products can be produced by conventionally known methods and common technical knowledge widely known to those skilled in the art. Examples of rubber products include tires, automotive rubber parts other than tires (exterior and interior parts, weatherstrips, boots, mounts, seals, sealers, gaskets), hoses, belts, sheets, vibration-isolating rubber, rollers, linings, rubber-coated fabrics, sealing materials, gloves, fenders, medical rubber (syringe gaskets, tubes, catheters), gaskets (for home appliances and construction), asphalt modifiers, grips, toys, shoes, sandals, keypads, gears, and PET bottle cap liners. Among these, tires are preferred.
[0091] [Tire] For example, a tire can be manufactured by extruding a polymer composition, molding it using a tire building machine, and then heating and pressurizing it using a vulcanizer to form crosslinks. The shape, structure, size, and material of the tire are not particularly limited and can be appropriately selected depending on the purpose. The use of the tire is also not particularly limited, and examples include passenger car tires, heavy duty tires, motorcycle tires, and studless tires. Tires manufactured using the polymer composition of the present invention have high grip performance and high breaking strength.
[0092] The polymer composition of the present invention can be applied to various parts of a tire. The part of a tire to which the polymer composition of the present invention is applied is not particularly limited, and can be appropriately selected depending on the purpose, such as a tire tread, a sidewall, a carcass, an inner liner, an undertread, or a belt part. Among these, the tire tread and a sidewall are particularly suitable.
[0093] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these examples. In the examples and comparative examples, "parts" and "%" are by mass unless otherwise specified. The methods for measuring various physical properties of polymers and rubbers are shown below.
[0094] (1) Bound styrene content (%, equivalent to the content of structural units derived from aromatic vinyl compounds): Deuterated chloroform was used as a solvent, and a 500 MHz 1 These were calculated by H-NMR measurement. (2) Content of short aromatic vinyl compound chains: and (3) Content of long aromatic vinyl compound chains: According to the method of Tanaka et al. [Polymer, 22, 1721 (1981)], styrene-butadiene copolymer rubber was decomposed with ozone, and then measurement was carried out under the following conditions using a gel permeation chromatography (GPC) apparatus "Alliance HPLC" (manufactured by Waters Corporation). The molecular weight in terms of polystyrene was determined from the retention time corresponding to the peak apex of the obtained GPC curve (for each peak if multiple peaks were present), and the number of styrene sequences corresponding to the peak was determined. In addition, the content of short aromatic vinyl compound chains and the content of long aromatic vinyl compound chains were calculated from the area ratio of each peak. (GPC conditions) Column: two columns of product name "GPC KF-801" (manufactured by Resonac) Column temperature: 40°C Mobile phase: tetrahydrofuran Flow rate: 0.6 ml / min Sample concentration: 0.2 wt% (4) Vinyl group content (%): 500 MHz 1 It was calculated by H-NMR measurement. (5) Weight average molecular weight of polymer: Measurement was carried out under the following conditions using a gel permeation chromatography (GPC) apparatus "HLC-8120GPC" (manufactured by Tosoh Corporation), and the weight average molecular weight (Mw) in terms of polystyrene was determined from the retention time corresponding to the maximum peak apex of the obtained GPC curve. (GPC conditions) Column: Trade name "GMHXL" (manufactured by Tosoh Corporation), 2 columns Column temperature: 40°C Mobile phase: tetrahydrofuran Flow rate: 1.0 ml / min Sample concentration: 10 mg / 20 ml
[0095] <Production Example of Conjugated Diene Polymer (A-1)> (Styrene Butadiene Rubber (SSBR) 1) A nitrogen-purged 5-liter autoclave reactor was charged with 2,000 g of cyclohexane, 2.5 mL of tetrahydrofuran as a vinyl content adjuster, 0.08 mmol of potassium 4-dodecylbenzenesulfonate as a potassium compound, and 175 g of styrene and 150 g of 1,3-butadiene as polymerization monomers. The temperature of the reactor contents was adjusted to 35°C, and then 3.7 mmol of n-butyllithium was added as a polymerization initiator to initiate polymerization. When the polymerization conversion reached 20% (corresponding to the point when the temperature of the contents reached 45°C), 175 g of 1,3-butadiene (additional amount) was added to the reactor at a constant feed rate over 25 minutes. The polymerization was carried out under adiabatic conditions, and the maximum temperature reached 85°C. When the polymerization conversion rate reached 99% (35 minutes after the start of polymerization), 3.7 mmol of 3-(N,N-bistrimethylsilyl)aminopropylmethyldiethoxysilane was added as a terminal modifier, and the mixture was stirred for 10 minutes. After stirring, 4.40 g of 2,6-di-tert-butyl-p-cresol was added as an antioxidant to the polymer solution, followed by steam stripping to remove the solvent and drying with a heated roll adjusted to 130°C to obtain a modified conjugated diene polymer (hereinafter also simply referred to as "styrene butadiene rubber (SSBR) 1").
[0096] (Styrene-Butadiene Rubber (SSBR) 2) A nitrogen-purged 50-liter autoclave reactor (first reactor) was continuously charged with 83 g / min of 1,3-butadiene as a monomer, 28 g / min of styrene, 745 g / min of cyclohexane as a solvent, 1.2 g / min of tetrahydrofuran as a vinyl group content adjuster (randomizer), and 55 mg / min of n-butyllithium as a polymerization initiator, and the temperature inside the reactor was controlled at 75°C. The polymer solution was continuously decharged from the first reactor at a rate of 860 g / min, and a compound represented by the following formula (N-Si-1) was added to the decharged polymer solution at a rate of 115 mg / min, and the compound was continuously introduced into the second reactor and reacted. At the outlet of the second reactor, di-tert-butyl-p-cresol was added so that the amount was 0.88 parts by mass per 100 parts by mass of the polymer. The solvent was removed from the polymer solution produced in this manner by steam stripping, and the resulting mixture was dried using a heated roll adjusted to 130°C to obtain a modified conjugated diene polymer (hereinafter also simply referred to as "styrene butadiene rubber (SSBR) 2").
[0097] (Styrene-Butadiene Rubber (SSBR) 3) A 5-liter autoclave reactor purged with nitrogen was charged with 2,000 g of cyclohexane, 5.6 mL of tetrahydrofuran as a vinyl content adjuster, and 175 g of styrene and 150 g of 1,3-butadiene as polymerization monomers. The temperature of the reactor contents was adjusted to 45°C, and then 3.7 mmol of n-butyllithium was added as a polymerization initiator to initiate polymerization. When the polymerization conversion reached 20% (corresponding to the point when the temperature of the contents reached 60°C), 175 g of 1,3-butadiene (additional amount) was added to the reactor at a constant feed rate over 25 minutes. The polymerization was carried out under adiabatic conditions, and the maximum temperature reached 85°C. When the polymerization conversion reached 99% (35 minutes after the start of polymerization), 3.7 mmol of 3-(N,N-bistrimethylsilyl)aminopropylmethyldiethoxysilane as a terminal modifier was added, and the mixture was stirred for 10 minutes. To the stirred polymer solution, 4.40 g of 2,6-di-tert-butyl-p-cresol was added as an antioxidant, and the solvent was then removed by steam stripping. The resulting mixture was then dried using a heated roll adjusted to 130°C, thereby obtaining a modified conjugated diene polymer (hereinafter, also simply referred to as "styrene butadiene rubber (SSBR) 3").
[0098] (Styrene-Butadiene Rubber (SSBR) 4) A 5-liter autoclave reactor purged with nitrogen was charged with 2,000 g of cyclohexane, 0.23 mmol of 2,2-di(2-tetrahydrofuryl)propane as a vinyl content adjuster, 0.15 mmol of potassium 4-dodecylbenzenesulfonate as a potassium compound, and 125 g of styrene and 200 g of 1,3-butadiene as polymerization monomers. After adjusting the temperature of the reactor contents to 40°C, 3.7 mmol of n-butyllithium as a polymerization initiator was added to initiate polymerization. When the polymerization conversion reached 20% (corresponding to the point when the temperature of the contents reached 50°C), 175 g of 1,3-butadiene (additional amount) was added to the reactor at a constant feed rate over 25 minutes. The polymerization was carried out under adiabatic conditions, and the maximum temperature reached 85°C. When the polymerization conversion rate reached 99% (35 minutes after the start of polymerization), 3.7 mmol of 3-(N,N-bistrimethylsilyl)aminopropylmethyldiethoxysilane was added as a terminal modifier, and the mixture was stirred for 10 minutes. After stirring, 4.40 g of 2,6-di-tert-butyl-p-cresol was added as an antioxidant to the polymer solution, followed by steam stripping to remove the solvent and drying with a heated roll adjusted to 130°C to obtain a modified conjugated diene polymer (hereinafter also referred to simply as "styrene butadiene rubber (SSBR) 4").
[0099] (Styrene-Butadiene Rubber (SSBR) 5) A 5-liter autoclave reactor purged with nitrogen was charged with 2,000 g of cyclohexane, 1.5 mL of tetrahydrofuran as a vinyl content adjuster, and 100 g of styrene and 180 g of 1,3-butadiene as polymerization monomers. The temperature of the reactor contents was adjusted to 75°C, and then 3.0 mmol of n-butyllithium as a polymerization initiator was added to initiate polymerization. When the polymerization conversion reached 20% (corresponding to 5 minutes after the start of the reaction), 120 g of 1,3-butadiene (additional amount) was added to the reactor at a constant feed rate over 30 minutes. The polymerization was carried out under isothermal conditions, and the maximum temperature reached 85°C. When the polymerization conversion reached 99% (35 minutes after the start of polymerization), 3.0 mmol of 3-(N,N-bistrimethylsilyl)aminopropylmethyldiethoxysilane as a terminal modifier was added, and the mixture was stirred for 10 minutes. To the stirred polymer solution, 3.52 g of 2,6-di-tert-butyl-p-cresol was added as an antioxidant, and the solvent was then removed by steam stripping. The resulting mixture was then dried using a heated roll adjusted to 130°C, yielding a modified conjugated diene polymer (hereinafter, also simply referred to as "styrene butadiene rubber (SSBR) 5").
[0100] Details of SSBR1 to 5 obtained above are shown in Table 1 below.
[0101] <Preparation of Raw Material Component Polymers> The following resins 1 to 7 were prepared. Resin 1 (manufactured by ENEOS Corporation, trade name: Neopolymer 150, unhydrogenated aromatic hydrocarbon resin, feedstock: aromatic olefin-containing C9 fraction) Resin 2 (manufactured by ENEOS Corporation, trade name: Neopolymer 140, unhydrogenated aromatic hydrocarbon resin, feedstock: aromatic olefin-containing C9 fraction) Resin 3 (manufactured by ENEOS Corporation, trade name: Neopolymer 130, unhydrogenated aromatic hydrocarbon resin, feedstock: aromatic olefin-containing C9 fraction) Resin 4 (manufactured by ENEOS Corporation, trade name: Neopolymer 120, unhydrogenated aromatic hydrocarbon resin, feedstock: aromatic olefin-containing C9 fraction) Resin 5 (manufactured by ENEOS Corporation, trade name: Neopolymer L90, unhydrogenated aromatic hydrocarbon resin, feedstock: aromatic olefin-containing C9 fraction) Resin 6 (manufactured by ENEOS Corporation, trade name: Neopolymer Premium 130S, unhydrogenated aromatic hydrocarbon resin, feedstock: aromatic olefin-containing C9 fraction) Resin 7 (manufactured by ENEOS Corporation, product name: Neopolymer Premium S100, unhydrogenated aromatic hydrocarbon resin, raw material: aromatic olefin-containing C9 fraction)
[0102] <Resin Evaluation> (Measurement of Number Average Molecular Weight (Mn)) Each of the above resins was dissolved in tetrahydrofuran to a concentration of 10 g / L to prepare a sample, and a Tosoh HLC-8320GPC (column used: TSKgel Super HZ column series) was used for measurement. The number average molecular weight Mn was calculated from the obtained RI curve using a calibration curve previously prepared using an Agilent polystyrene kit (EasiVial PS-M and PS-L). The calculation results are shown in Table 2.
[0103] (Measurement of proton amount) The proton amount of each of the above resins was measured by the following measurement procedures 1 to 3. The measurement results are shown in Table 2. 1. A sample prepared by dissolving 10 mg of resin and 5.5 mg of a standard substance (dimethyl terephthalate) in 1 g of deuterated chloroform was 1 1 H NMR was measured. The standard substance was selected so that its peak did not overlap with the aromatic region of the resin. 2. The number of aromatic protons in the sample was quantified by the internal standard method. Based on the amount charged, the sample contained 2.5 × 10 -5The resin contained approximately 100 mol of dimethyl terephthalate. The integral value of the internal standard aromatic ring proton (4H) was set to 1.00, and the corresponding proton amount was calculated from the integral values of the resin's olefin region (4.5-6.0 ppm) and aromatic region (6.0-7.5 ppm). Furthermore, the influence of protons derived from residual deuterated chloroform, which overlap with the aromatic region, can be ignored by subtracting the value obtained by a blank measurement using a resin-free sample. 3. The number of aromatic protons contained in one molecule was calculated from the Mn of each resin calculated above.
[0104]
[0105] Test Example 1 Example 1 The following components were kneaded using a 250 mL kneader (Labo Plastomill B250 manufactured by Toyo Seiki Seisakusho, Ltd.) to obtain a polymer composition. The kneading conditions were a temperature of 70°C, a rotation speed of 50 rpm, and a kneading time of 0.5 minutes for masticating the rubber component, followed by 1.5 minutes of kneading after adding silica and additives, and then 2 minutes of kneading (the rubber temperature during kneading was maintained at 150°C). SSBR1 60 parts by mass SSBR2 40 parts by mass Silica (manufactured by Solvay, trade name: 1165MP) 70 parts by mass Carbon black (manufactured by Tokai Carbon Co., Ltd., trade name: Seest KH) 5.60 parts by mass Zinc oxide No. 3 (manufactured by Toho Zinc Co., Ltd., trade name: Ginrei R) 3 parts by mass Stearic acid (manufactured by New Japan Chemical Co., Ltd., trade name: Stearic Acid 300) 2 parts by mass Antiaging agent (manufactured by Ouchi Shinko Chemical Co., Ltd., trade name: Nocrac 6C) 1 part by mass Silane coupling agent (manufactured by Evonik Corporation, trade name: Si75) 5.60 parts by mass Resin 1 15.0 parts by mass Sulfur (manufactured by Hosoi Chemical Co., Ltd., trade name: Oil Sulfur 325 mesh (5%)) 1.20 parts by mass Vulcanization accelerator 1 (manufactured by Ouchi Shinko Chemical Co., Ltd., trade name: Noccela CZ) 1.44 parts by mass Vulcanization accelerator 2 (manufactured by Ouchi Shinko Chemical Co., Ltd., product name: Noccela D) 1.20 parts by mass
[0106] Example 2 A polymer composition was obtained in the same manner as in Example 1, except that 15.0 parts by mass of Resin 2 was added instead of Resin 1.
[0107] Example 3 A polymer composition was obtained in the same manner as in Example 1, except that 15.0 parts by mass of Resin 3 was added instead of Resin 1.
[0108] Example 4 A polymer composition was obtained in the same manner as in Example 1, except that 15.0 parts by mass of Resin 4 was added instead of Resin 1.
[0109] Example 5 A polymer composition was obtained in the same manner as in Example 1, except that 15.0 parts by mass of Resin 5 was added instead of Resin 1.
[0110] Example 6 A polymer composition was obtained in the same manner as in Example 1, except that 15.0 parts by mass of Resin 6 was added instead of Resin 1.
[0111] Comparative Example 1 A polymer composition was obtained in the same manner as in Example 1, except that 15.0 parts by mass of aromatic oil (T-DAE, manufactured by ENEOS Corporation) was added instead of Resin 1.
[0112] Comparative Example 2 A polymer composition was obtained in the same manner as in Example 1, except that 15.0 parts by mass of Resin 8 (unhydrogenated petroleum resin, raw material: containing C5 fraction and C9 fraction, manufactured by Tosoh Corporation, product name: Petrotack 100V, number average molecular weight (Mn) 955) was added instead of Resin 1.
[0113] Comparative Example 3 A polymer composition was obtained in the same manner as in Example 1, except that 15.0 parts by mass of Resin 9 (a homo-oligomer of α-methylstyrene, manufactured by Cray Valley, product name: W-140, number average molecular weight (Mn) 1701) was added instead of Resin 1.
[0114] [Physical Property Evaluation] (Viscoelasticity) Each of the polymer compositions obtained above was heated and pressed for 30 minutes at 160°C and 20 MPa using a mold (manufactured by Dumbbell, model number: MP-124NJ) to obtain a rubber sheet (thickness: 2 mm, length: 150 mm, width: 150 mm). Subsequently, the tan δ of the obtained rubber sheet was measured at a measurement temperature of 0°C using a viscoelasticity measuring device (manufactured by UBM, Rheogel E-4000) in accordance with JIS K6394 under conditions of a strain of 20 μm (approximately 0.1%) and a frequency of 10 Hz. The measurement results are shown in Table 3. A larger value of tan δ (0°C) indicates better gripping properties. Regarding the tan δ results for Examples 1 to 6 and Comparative Examples 1 and 3, the values were reported as relative values, with the value for Comparative Example 2 being set at 100.
[0115] (Tensile Properties) Rubber sheets were obtained in the same manner as in the viscoelasticity test described above. No. 3 dumbbell-shaped test pieces were punched out from the obtained rubber sheets, and the breaking strength (MPa) and breaking elongation (%) were measured at a temperature of 25°C and a tensile speed of 500 mm / min in accordance with JIS K6251 (issued in 2010). From these measurement results, the tensile product (=breaking strength × breaking elongation) was calculated. The calculation results are shown in Table 3. A higher tensile product indicates better breaking strength. Note that the tensile product results for Examples 1 to 6 and Comparative Examples 1 and 3 are reported as relative values, with the value for Comparative Example 2 being set at 100.
[0116]
[0117] Test Example 2 Example 7 A polymer composition was obtained in the same manner as in Example 1, except that 15.0 parts by mass of Resin 7 was added instead of Resin 1.
[0118] Example 8 A polymer composition was obtained in the same manner as in Example 7, except that 7 parts by mass of SSBR1, 40 parts by mass of SSBR2, and 53 parts by mass of SSBR3 were added as the styrene-butadiene rubber.
[0119] Comparative Example 4 A polymer composition was obtained in the same manner as in Example 7, except that 40 parts by mass of SSBR2 and 60 parts by mass of SSBR3 were added as the styrene-butadiene rubber.
[0120] [Evaluation of Physical Properties] (Viscoelasticity) Rubber sheets were obtained using each polymer composition in the same manner as in Test Example 1. Subsequently, tan δ at a measurement temperature of 0°C was determined for the obtained rubber sheets. The measurement results are shown in Table 4. Note that the tan δ results for Examples 7 and 8 were reported as relative values when the value for Comparative Example 4 was set to 100.
[0121] (Tensile Properties) A rubber sheet was obtained in the same manner as in the viscoelasticity test described above. Subsequently, the breaking strength (MPa) and breaking elongation (%) of the obtained rubber sheet were measured in the same manner as in Test Example 1. From these measurement results, the tensile product (=breaking strength × breaking elongation) was calculated. The calculation results are shown in Table 4. Note that the tensile product results for Examples 7 and 8 are shown as relative values, with the value for Comparative Example 4 being set at 100.
[0122]
[0123] Test Example 3 Example 9 A polymer composition was obtained in the same manner as in Example 7, except that 40 parts by mass of SSBR2 and 60 parts by mass of SSBR4 were added as the styrene-butadiene rubber.
[0124] Comparative Example 5 A polymer composition was obtained in the same manner as in Example 9, except that 40 parts by mass of SSBR2 and 60 parts by mass of SSBR5 were added as the styrene-butadiene rubber.
[0125] [Physical Property Evaluation] (Viscoelasticity) Rubber sheets were obtained using each polymer composition in the same manner as in Test Example 1. Subsequently, tan δ at a measurement temperature of 0°C was determined for the obtained rubber sheets. The measurement results are shown in Table 5. Note that, for each tan δ result for Example 9, the value for Comparative Example 5 was set to 100, and the result was reported as a relative value.
[0126] (Tensile Properties) A rubber sheet was obtained in the same manner as in the viscoelasticity test described above. Subsequently, the breaking strength (MPa) and breaking elongation (%) of the obtained rubber sheet were measured in the same manner as in Test Example 1. From these measurement results, the tensile product (=breaking strength × breaking elongation) was calculated. The calculation results are shown in Table 5. Note that the tensile product results for Example 9 are shown as relative values, with the value for Comparative Example 5 being set at 100.
[0127]
[0128] <Test Example 4> [Example 10] A polymer composition was obtained in the same manner as in Example 3, except that the amount of silica added was changed to 100 parts by mass, the amount of silane coupling agent added was changed to 8.0 parts by mass, and the amount of resin 3 added was changed to 40.0 parts by mass.
[0129] Comparative Example 6 A polymer composition was obtained in the same manner as in Example 10, except that 40.0 parts by mass of Resin 10 was added instead of Resin 3.
[0130] [Physical Property Evaluation] (Viscoelasticity) Rubber sheets were obtained using each polymer composition in the same manner as in Test Example 1. Subsequently, tan δ at a measurement temperature of 0°C was determined for the obtained rubber sheets. The measurement results are shown in Table 6. Note that, for each result of tan δ, the value for Example 10 was shown as a relative value when the value for Comparative Example 6 was set to 100.
[0131] (Tensile Properties) A rubber sheet was obtained in the same manner as in the viscoelasticity test described above. Subsequently, the breaking strength (MPa) and breaking elongation (%) of the obtained rubber sheet were measured in the same manner as in Test Example 1. From these measurement results, the tensile product (=breaking strength × breaking elongation) was calculated. The calculation results are shown in Table 6. Note that the tensile product results for Example 10 were reported as relative values, with the value for Comparative Example 6 being set at 100.
[0132]
Claims
1. A polymer composition comprising: a rubber component containing a conjugated diene polymer (A-1); and a raw material component polymer of a C9 fraction containing an aromatic olefin, wherein the conjugated diene polymer (A-1) contains structural units derived from a conjugated diene compound and structural units derived from an aromatic vinyl compound, the content of the structural units derived from the aromatic vinyl compound is 5% by mass or more and 60% by mass or less based on the total amount of the structural units derived from the conjugated diene compound and the structural units derived from the aromatic vinyl compound, and the content of the structural units derived from the aromatic vinyl compound is less than 40% by mass of aromatic vinyl compound single chains in which aromatic vinyl compounds are not consecutive, and is 10% by mass or less of aromatic vinyl compound long chains in which 8 or more aromatic vinyl compound units are linked together.
2. The polymer composition according to claim 1, wherein the aromatic olefin-containing C9 fraction comprises at least one member selected from the group consisting of vinyltoluene, α-methylstyrene, styrene, indene, and methylindene.
3. The polymer composition according to claim 1, wherein the amount of protons per molecule of the raw material component polymer satisfies the following conditions: 0<aromatic proton amount≦1000 0≦olefinic proton amount≦45.
4. The polymer composition according to claim 1, wherein the number average molecular weight (Mn) of the raw material component polymer is 300 g / mol or more and less than 3,000 g / mol.
5. The polymer composition according to claim 1, wherein the content of the conjugated diene polymer (A-1) is 5 mass % or more of the total amount of the rubber component.
6. The polymer composition according to claim 1, wherein the conjugated diene polymer (A-1) has a nitrogen-containing group and a hydrocarbyloxysilyl group.
7. The polymer composition of claim 1 further comprising a filler.
8. A rubber product formed using the polymer composition according to any one of claims 1 to 7.
9. The rubber article of claim 8, wherein said rubber article is selected from the group consisting of tires, tire treads, and sidewalls.
Citation Information
Patent Citations
Rubber composition for tire and pneumatic tire
JP2011140613A
Elastomeric blend for tires comprising high glass transition temperature hydrocarbon resins
JP2018193567A
Rubber composition containing hydrocarbon resin
JP2018536044A
Rubber composition
JP2009108193A
Modified conjugated diene-based polymer composition, rubber composition and method for producing rubber composition
JP2020033549A