Adhesive sheet, adhesive sheet with release film, laminate for image display device, image display device, and adhesive sheet for image display device component

The adhesive sheet with a tailored acrylic copolymer layer and release film ensures reliable bonding at the edges of image display devices, addressing air bubble and adhesive oozing issues, enhancing the appearance and functionality of narrow frame designs.

WO2024203789A1PCT designated stage expired Publication Date: 2024-10-03MITSUBISHI CHEM CORP

Patent Information

Application Number
PCT/JP2024/011178
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional adhesive sheets for image display devices face challenges in achieving high bonding reliability at the peripheral edges, particularly in narrow frame designs, where air bubbles and adhesive oozing are common due to the lack of appropriate hardness and flexibility, leading to reduced visibility and design limitations.

Method used

A pressure-sensitive adhesive sheet with an acrylic copolymer layer, specifically designed to have a stress relaxation rate of 0.25 or more, an initial elastic modulus between 5 to 100 kPa, and a gel fraction of 30 to 95%, which is laminated with a release film to ensure bubble-free bonding up to the peripheral edge, addressing the issues of adhesive oozing and edge reliability.

Benefits of technology

The adhesive sheet provides enhanced bonding reliability and resistance to air bubbles at the peripheral edges, enabling the use in narrow frame designs and frameless displays without compromising adhesive strength or flexibility, thus improving the overall appearance and functionality of image display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

The purpose is to provide an adhesive sheet having a higher level of lamination reliability than in the past. Provided is an adhesive sheet having an acrylic adhesive layer formed from an adhesive composition containing an acrylic copolymer (A), wherein the acrylic adhesive layer has a stress relaxation rate, calculated by formula (I) from the initial modulus (G'(0)) 0.1 second after applying 25% strain at a temperature of 70°C and the relaxation modulus (G'(300)) 300 seconds after applying 25% strain at a temperature of 70°C, of 0.25 or more. Stress relaxation rate=(G'(300) / G'(0))... (I)
Need to check novelty before this filing date? Find Prior Art

Description

Adhesive sheet, adhesive sheet with release film, laminate for image display device, image display device, and adhesive sheet for image display device constituent member

[0001] The present invention relates to a pressure-sensitive adhesive sheet, a pressure-sensitive adhesive sheet with a release film, a laminate for an image display device, an image display device, and a pressure-sensitive adhesive sheet for a component of an image display device.

[0002] In order to improve the visibility of image display devices, the gap between an image display panel such as a liquid crystal display (LCD), a plasma display (PDP), or an electroluminescence display (ELD) and a protective panel or touch panel member placed on the front side (viewing side) of the image display panel is filled with a resin such as an adhesive or glue, thereby suppressing reflection of incident light and outgoing light from the displayed image at the air layer interface.

[0003] For example, Patent Document 1 discloses a method for manufacturing a component laminate for an image display device, which has a configuration in which an image display device component is laminated on at least one side of a transparent double-sided adhesive sheet, in which an adhesive sheet that has been primarily crosslinked by ultraviolet light is attached to the image display device component, and then the adhesive sheet is irradiated with ultraviolet light through the image display device component to cause secondary curing.

[0004] Furthermore, Patent Document 2 discloses a pressure-sensitive adhesive sheet containing a (meth)acrylic copolymer having an ultraviolet-crosslinkable site, as a pressure-sensitive adhesive sheet useful for displays and touch panels.

[0005] Patent No. 4971529 Patent No. 6062740

[0006] There is a strong demand for image display devices to have as large an effective display area as possible without changing the external dimensions, i.e., to have a narrower frame. For this reason, there is also a demand for adhesive sheets for bonding image display components that can bond without air bubbles, even to the peripheral edge near the edge of the adhesive sheet, which in the past was located directly below the concealing part and was therefore not visible.

[0007] Furthermore, in recent years, there has been a demand for high design quality in image display devices, and the shape of the front surface protection panel is changing from flat to those with curved edges or corners, or to designs in which the entire display unit is curved, etc. In the case of curved members or members with curved edges or corners, air bubbles are more likely to occur around the periphery than in flat members.

[0008] The pressure-sensitive adhesive sheets in Patent Documents 1 and 2 were developed for laminated structures using conventional image display device components, and did not take into consideration the lamination reliability near the peripheral edge of the pressure-sensitive adhesive sheet, which would have been located directly below the concealed portion and therefore not visible in conventional cases. Furthermore, conventional flexible pressure-sensitive adhesive sheets tend to have crushed edges and the glue (adhesive layer) easily overflows. To address this issue, a certain degree of hardness is desirable, but excessive hardness can lead to the problem of air bubbles forming around the edges. Therefore, for image display devices with increasingly narrower picture frames, pressure-sensitive adhesive sheets that have an appropriate hardness yet offer better lamination reliability at the peripheral edge, which is a trade-off.

[0009] Therefore, in this context, the present invention provides an adhesive sheet, an adhesive sheet with a release film, a laminate for an image display device, an image display device, and an adhesive sheet for a component of an image display device, which have a higher level of bonding reliability than conventional ones.

[0010] That is, the present invention has the following aspects: [1] A pressure-sensitive adhesive sheet having an acrylic pressure-sensitive adhesive layer formed from a pressure-sensitive adhesive composition containing an acrylic copolymer (A), wherein the acrylic pressure-sensitive adhesive layer has a stress relaxation rate of 0.25 or more, calculated by the following formula (I) from the initial elastic modulus (G'(0)) 0.1 second after applying a 25% strain at a temperature of 70°C to the acrylic pressure-sensitive adhesive layer and the relaxation elastic modulus (G'(300)) 300 seconds after applying a 25% strain at a temperature of 70°C to the acrylic pressure-sensitive adhesive layer: Stress relaxation rate=(G'(300) / G'(0)) (I) [2] A pressure-sensitive adhesive sheet having an acrylic pressure-sensitive adhesive layer, wherein the acrylic pressure-sensitive adhesive layer is a cured reaction product formed from a syrup composition comprising an alkyl(meth)acrylate (a1) having an alkyl group containing 3 to 30 carbon atoms and a hydroxyl group-containing (meth)monomer (a2), and wherein the stress relaxation rate calculated by the following formula (I) from the initial elastic modulus (G'(0)) 0.1 second after applying a 25% strain at a temperature of 70°C to the acrylic pressure-sensitive adhesive layer and the relaxed elastic modulus (G'(300)) 300 seconds after applying a 25% strain at a temperature of 70°C to the acrylic pressure-sensitive adhesive layer is 0.25 or more. Stress relaxation rate=(G'(300) / G'(0)) (I) [3] The pressure-sensitive adhesive sheet according to [1] or [2], wherein the initial elastic modulus (G'(0)) is 5 to 100 kPa. [4] The pressure-sensitive adhesive sheet according to any one of [1] to [3], wherein the relaxation modulus (G'(300)) is 1.3 to 100 kPa. [5] The pressure-sensitive adhesive sheet according to any one of [1] to [4], wherein the gel fraction of the pressure-sensitive adhesive sheet is 30 to 95%. [6] The pressure-sensitive adhesive sheet according to any one of [1] to [5], wherein the storage modulus (G'(25°C)) at a temperature of 25°C, obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz, is 80 kPa or more. [7] The pressure-sensitive adhesive sheet according to any one of [1] to [6], wherein the glass transition temperature (Tg), defined as the maximum value of Tan δ, obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz, is -20°C or more. [8] The pressure-sensitive adhesive sheet according to any one of [1] to [7], wherein the pressure-sensitive adhesive sheet is a single layer. [9] The pressure-sensitive adhesive sheet according to [1], wherein the pressure-sensitive adhesive composition contains a crosslinking agent (B) and a photoinitiator (C).

[10] The pressure-sensitive adhesive sheet according to [9], wherein the photoinitiator (C) comprises a photoinitiator (c1) having, in its molecule, a radical-polymerizable functional group having a carbon-carbon double bond and a structure that generates a radical, and a hydrogen-abstraction photoinitiator (c2) other than the photoinitiator (c1).

[11] A pressure-sensitive adhesive sheet with a release film, comprising the pressure-sensitive adhesive sheet according to any one of [1] to

[10] and a release film laminated on the pressure-sensitive adhesive sheet.

[12] A laminate for an image display device, comprising two image display device components and the pressure-sensitive adhesive sheet according to any one of [1] to

[10] interposed between the two image display device components, wherein one of the two image display device components is a surface protection panel, and the other is a member comprising any one or a combination of two or more selected from the group consisting of a touch sensor film, an image display panel, a color filter, a polarizing element, and a retardation film.

[13] The laminate for an image display device according to

[12] , wherein the surface protection panel has a frame-shaped concealing portion on its periphery, and the concealing portion has a portion with a frame width of 3 mm or less.

[14] The laminate for an image display device according to

[12] or

[13] , which is fixed in a curved state.

[15] An image display device comprising the laminate for an image display device according to any one of

[12] to

[14] .

[16] A pressure-sensitive adhesive sheet for a component of an image display device, comprising the pressure-sensitive adhesive sheet according to any one of [1] to

[10] .

[0011] The pressure-sensitive adhesive sheet of the present invention can be attached without bubbles even to the peripheral edge near the edge of the pressure-sensitive adhesive sheet, which in conventional cases was located directly below the concealing portion and was therefore not visible. Therefore, the pressure-sensitive adhesive sheet can be suitably used as a pressure-sensitive adhesive sheet for image display devices, particularly image display devices with narrow frame designs or frameless designs.

[0012] An example of an embodiment of the present invention will be described in detail below. However, the present invention is not limited to the embodiment described below. In this specification, the term "film" conceptually includes a sheet, a film, and a tape. Furthermore, when the term "panel" is used, such as an image display panel or a protective panel, it includes a plate, a sheet, and a film.

[0013] In this specification, when it is stated that "x to y" (x and y are any numbers), it means "x or more and y or less" unless otherwise specified, and also includes the meaning of "preferably greater than x" or "preferably smaller than y." Furthermore, when it is stated that "x or more" (x is any number), it also includes the meaning of "preferably greater than x" unless otherwise specified, and when it is stated that "y or less" (y is any number), it also includes the meaning of "preferably smaller than y" unless otherwise specified. Furthermore, "x and / or y (x and y are any configurations)" means at least one of x and y, and can mean three possibilities: x only, y only, or x and y. Furthermore, in this specification, "(meth)acrylic" means a comprehensive definition of acrylic and methacrylic, "(meth)acrylate" means a comprehensive definition of acrylate and methacrylate, and "(meth)acryloyl" means a comprehensive definition of acryloyl and methacryloyl. Furthermore, in this specification, the term "major component" refers to a component that has a significant effect on the properties of the material, and the content of that component is usually 50% by mass or more, preferably 70% by mass or more, and particularly preferably 90% by mass or more, of the entire material. Furthermore, with regard to the numerical ranges described in stages in this specification, the upper or lower limit of a certain numerical range can be arbitrarily combined with the upper or lower limit of another numerical range. Furthermore, in the numerical ranges described in this specification, the upper or lower limit of the numerical range can also be replaced with the values ​​shown in the examples.

[0014] <<Adhesive Sheet>> A pressure-sensitive adhesive sheet according to one example of an embodiment of the present invention (hereinafter referred to as "the present pressure-sensitive adhesive sheet 1") is a pressure-sensitive adhesive sheet having an acrylic pressure-sensitive adhesive layer formed from a pressure-sensitive adhesive composition containing an acrylic polymer (A), wherein the acrylic pressure-sensitive adhesive layer has a stress relaxation rate of 0.25 or more, as calculated by the following formula (I) from the initial elastic modulus (G'(0)) 0.1 second after applying a 25% strain at a temperature of 70°C and the relaxation elastic modulus (G'(300)) 300 seconds after applying a 25% strain at a temperature of 70°C:

[0023] Stress relaxation rate = (G'(300) / G'(0)) (I)

[0024] Furthermore, a pressure-sensitive adhesive sheet according to one example of a second embodiment of the present invention (hereinafter referred to as "Present Pressure-sensitive Adhesive Sheet 2") is a pressure-sensitive adhesive sheet having an acrylic pressure-sensitive adhesive layer, wherein the acrylic pressure-sensitive adhesive layer is a cured reaction product formed from a syrup composition comprising an alkyl (meth)acrylate (a1) having an alkyl group with 3 or more carbon atoms and a hydroxyl group-containing (meth)acrylate (a2), and the pressure-sensitive adhesive layer has a stress relaxation rate (X0) of 0.25 or more, as calculated by the following formula (I) from the initial modulus of elasticity (G0'(0)) 0.1 second after application of a 25% strain at a temperature of 70°C and the relaxed modulus of elasticity (G0'(300)) 300 seconds after application. Stress relaxation rate (X0) = (G0'(300) / G0'(0)) (I)

[0025] Present Pressure-sensitive Adhesive Sheet 1 and Present Pressure-sensitive Adhesive Sheet 2 will now be described. Furthermore, the present pressure-sensitive adhesive sheet 1 and the present pressure-sensitive adhesive sheet 2 may be collectively referred to simply as "the present pressure-sensitive adhesive sheet."

[0015] This pressure-sensitive adhesive sheet satisfies the following requirement (1): Requirement (1) The stress relaxation rate calculated from the initial elastic modulus (G'(0)) 0.1 seconds after applying a 25% strain at 70°C to the acrylic pressure-sensitive adhesive layer and the relaxation elastic modulus (G'(300)) 300 seconds after applying a 25% strain at 70°C using the following formula (I) is 0.25 or more: Stress relaxation rate = (G'(300) / G'(0)) (I)

[0016] A pressure-sensitive adhesive sheet that satisfies requirement (1) has high cohesive strength, and therefore air trapped during lamination is less likely to form bubbles, which can reduce or eliminate bubbles at the peripheral edge of the pressure-sensitive adhesive sheet.

[0017] In laminates requiring precision lamination, such as laminates for image display devices, finishing lamination is typically performed by heating and pressurizing using an autoclave when laminating components. After the autoclave process is completed or after the product begins to be used, air bubbles may form at the peripheral edges. One of the main causes of these bubbles is thought to be the infiltration of air present in the autoclave oven between the laminating components and the pressure-sensitive adhesive sheet due to the high pressure inside the oven during the lamination process. Conventionally, these air bubbles were not visible because the peripheral edges of displays were covered by a concealing layer such as a printed layer or a bezel. However, in recent years, due to demands for narrower display frames and frameless designs, the peripheral edges have become narrower, and there is a strong demand for improved bubble resistance at the peripheral edges of pressure-sensitive adhesive sheets.

[0018] From the viewpoint of improving the foaming resistance at the peripheral edge of the pressure-sensitive adhesive sheet, the stress relaxation rate is preferably 0.3 or more, more preferably 0.35 or more, even more preferably 0.4 or more, and even more preferably 0.45 or more, and particularly preferably 0.55 or more. On the other hand, the upper limit is usually 1, but from the viewpoint of obtaining an appropriate stress relaxation property, the stress relaxation rate is preferably 0.9 or less, more preferably 0.8 or less, and even more preferably 0.7 or less. The lower limit and upper limit of the stress relaxation rate can be combined arbitrarily.

[0019] The stress relaxation rate can be determined as follows: The initial elastic modulus (G'(0)) and the relaxation elastic modulus (G'(300)) are measured by the method described below, and the obtained values ​​are substituted into the following formula (I) to calculate the stress relaxation rate (X0)=(G'(300) / G'(0)) (I)

[0020] Examples of methods for adjusting the stress relaxation rate include, but are not limited to, methods for adjusting the composition and molecular weight of the acrylic polymer (A), the type and content of the crosslinking agent (B) and the photoinitiator (C), and methods for adjusting the amount of active energy ray irradiation.

[0021] The present pressure-sensitive adhesive sheet preferably further satisfies the following requirement (2): Requirement (2) The acrylic pressure-sensitive adhesive layer has an initial elastic modulus (G'(0)) of 5 to 100 kPa 0.1 seconds after a 25% strain is applied at 70°C.

[0022] A pressure-sensitive adhesive sheet satisfying requirement (2) has a moderate cohesive force, and therefore has excellent handleability. Furthermore, when a member is attached to the pressure-sensitive adhesive sheet, the peripheral edge of the pressure-sensitive adhesive sheet is less likely to be crushed, and adhesive extrusion at the edge tends to be reduced or eliminated. From the viewpoint of reducing adhesive extrusion, the initial modulus of elasticity (G'(0)) is preferably 10 kPa or more, more preferably 15 kPa or more, and even more preferably 20 kPa or more. Furthermore, when the adherend has irregularities, from the viewpoint of filling the surface irregularities during attachment, the initial modulus of elasticity (G'(0)) is preferably 60 kPa or less, more preferably 50 kPa or less, and even more preferably 40 kPa or less. The lower and upper limits of the initial modulus of elasticity (G'(0)) of requirement (2) can be arbitrarily combined.

[0023] The initial elastic modulus (G'(0)) is measured, for example, as follows: PSA sheets are repeatedly laminated to a thickness of 0.7 to 1.2 mm (for example, about 0.8 mm), and then punched out to a diameter of 8 mm. A strain of 25% is applied to the obtained sample at 70°C using a rheometer, and the elastic modulus is read after 0.1 seconds.

[0024] In measuring the initial modulus of elasticity (G'(0)), it is necessary to avoid fluctuations in the measurement results due to the influence of the measuring jig. The initial modulus of elasticity (G'(0)) is a value measured after adjusting the thickness to a range of 0.7 to 1.2 mm, which allows the initial modulus of elasticity (G'(0)) to be accurately measured without being affected by the measuring jig. Note that "adjusted to a thickness of 0.7 to 1.2 mm" means that if the thickness of the pressure-sensitive adhesive sheet used as the measurement sample does not fall within this range, the thickness of the measurement sample is adjusted to fall within this range by, for example, stacking several sheets. The same applies when the thickness of the measurement sample is specified in other tests.

[0025] Examples of methods for adjusting the initial elastic modulus (G'(0)) include a method for adjusting the composition or molecular weight of the acrylic polymer (A), or the type or amount of the crosslinking agent (B) or the photoinitiator (C), as well as a method for adjusting the amount of active energy ray irradiation, although the methods are not limited to these.

[0026] The present pressure-sensitive adhesive sheet preferably further satisfies the following requirement (3): Requirement (3) The acrylic pressure-sensitive adhesive layer has a relaxation modulus (G'(300)) of 1.3 to 100 kPa 300 seconds after a 25% strain is applied at 70°C.

[0027] A pressure-sensitive adhesive sheet satisfying requirement (3) has a moderate cohesive strength, and therefore has excellent handleability. Furthermore, when attached to a member, the peripheral edge of the pressure-sensitive adhesive sheet is less likely to be crushed, and adhesive extrusion at the edge tends to be reduced or eliminated. From the viewpoint of reducing adhesive extrusion, the relaxation modulus (G'(300)) is preferably 2 kPa or more, more preferably 5 kPa or more, and even more preferably 10 kPa or more. Furthermore, from the viewpoint of maintaining moderate flexibility and ensuring wettability to the adherend, the relaxation modulus (G0'(300)) is preferably 80 kPa or less, more preferably 70 kPa or less, even more preferably 60 kPa or less, and particularly preferably 50 kPa or less. The lower and upper limits of the relaxation modulus (G'(300)) can be arbitrarily combined.

[0028] The relaxation modulus (G'(300)) is measured, for example, as follows: PSA sheets are repeatedly laminated to a thickness of 0.7 to 1.2 mm (for example, about 0.8 mm), and then punched out to a diameter of 8 mm. A strain of 25% is applied to the obtained sample at 70°C using a rheometer, and the modulus is read after 300 seconds.

[0029] Examples of methods for adjusting the relaxation modulus (G'(300)) include, but are not limited to, methods for adjusting the composition and molecular weight of the acrylic polymer (A) and the type and content of the crosslinking agent (B) and photoinitiator (C), as well as methods for adjusting the amount of active energy ray irradiation.

[0030] It is preferable that the pressure-sensitive adhesive sheet further satisfies the following requirement (4): Requirement (4) The shear storage modulus (G'(25°C)) at 25°C, obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz, is 80 kPa or more.

[0031] PSA sheets that satisfy requirement (4) tend to have excellent handleability and resistance to adhesive extrusion. From this perspective, the shear storage modulus at 25°C (G'(25°C)) is preferably 100 kPa or more, more preferably 150 kPa or more, more preferably 200 kPa or more, even more preferably 250 kPa or more, particularly preferably 300 kPa or more, and even more preferably 400 kPa or more. On the other hand, from the viewpoint of ensuring the stress relaxation properties of the PSA sheet, the shear storage modulus at 25°C (G'(25°C)) is preferably 1000 kPa or less, more preferably 900 kPa or less, and even more preferably 800 kPa or less. The lower limit and upper limit of the shear storage modulus at 25°C (G'(25°C)) can be combined arbitrarily.

[0032] The shear storage modulus at 25°C (G'(25°C)) is measured, for example, as follows. PSA sheets are repeatedly laminated to adjust the thickness to 0.7 to 1.2 mm (for example, 0.8 mm), and then punched out into circles with a diameter of 8 mm. The obtained sample is subjected to dynamic viscoelasticity measurement using a rheometer under the conditions of a measuring jig: 8 mm diameter parallel plates, a frequency: 1 Hz, a measuring temperature: -50 to 150°C, and a heating rate: 5°C / min, and the value of the shear storage modulus at 25°C (G'(25°C)) is read.

[0033] Examples of a method for adjusting the shear storage modulus at 25°C (G'(25°C)) within the above range include a method for adjusting the composition or molecular weight of the acrylic polymer (A) or the type or content of the crosslinking agent (B) or the photoinitiator (C), as well as a method for adjusting the amount of active energy ray irradiation. However, the method is not limited to these methods.

[0034] The pressure-sensitive adhesive sheet preferably further satisfies the following requirement (5): Requirement (5) The glass transition temperature (Tg) defined as the maximum value of Tan δ obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz is −25° C. or higher.

[0035] PSA sheets that satisfy requirement (5) tend to have excellent handleability and adhesive extrusion resistance. From this viewpoint, the glass transition temperature (Tg) is preferably -20°C or higher, more preferably -15°C or higher, even more preferably -10°C or higher, particularly preferably -5°C or higher, and most preferably 0°C or higher. On the other hand, from the viewpoint of obtaining appropriate flexibility and stress relaxation, the upper limit is preferably 60°C or lower, more preferably 50°C or lower, and even more preferably 40°C or lower. The lower limit and upper limit of the glass transition temperature (Tg) can be combined arbitrarily.

[0036] The glass transition temperature (Tg) can be obtained by reading the temperature at which the loss tangent (Tan δ) becomes a maximum value, i.e., the peak temperature, from dynamic viscoelasticity spectrum data in shear mode obtained by the same measurement method as for the shear storage modulus (G'(25°C)) at 25°C described above. When there are multiple maximum values ​​in the viscoelasticity spectrum, the "peak temperature" refers to the temperature at which the largest maximum value is obtained.

[0037] Examples of a method for adjusting the glass transition temperature (Tg) within the above range include a method for adjusting the composition or molecular weight of the acrylic polymer (A) or the type or content of the crosslinking agent (B) or the photoinitiator (C), and a method for adjusting the amount of active energy ray irradiation, although the method is not limited to these.

[0038] It is preferable that the present pressure-sensitive adhesive sheet further satisfies the following requirement (6): Requirement (6) The gel fraction of the pressure-sensitive adhesive sheet is 30 to 90%.

[0039] A pressure-sensitive adhesive sheet satisfying requirement (6) has a moderate cohesive strength and tends to have excellent handleability and shape stability. From the viewpoint of obtaining a moderate cohesive strength, the gel fraction is preferably 35% or more, more preferably 40% or more, and even more preferably 45% or more. On the other hand, from the viewpoint of obtaining stress relaxation, the gel fraction is preferably 90% or less, more preferably 87% or less, and even more preferably 85% or less. The lower limit and upper limit of the gel fraction can be arbitrarily combined.

[0040] The gel fraction is measured, for example, as follows: A pre-measured mass of the pressure-sensitive adhesive sheet and a 150-mesh SUS wire mesh are prepared. The pressure-sensitive adhesive sheet is then wrapped in the SUS wire mesh and immersed in ethyl acetate at 23°C for 24 hours. The sheet is then dried at 70°C for 4.5 hours, and the mass of the sheet and the SUS wire mesh is measured. The mass of the insoluble pressure-sensitive adhesive sheet remaining in the wire mesh (mass after immersion) is determined by subtracting the mass of the SUS wire mesh from the mass of the pressure-sensitive adhesive sheet before immersion in ethyl acetate (mass before immersion). The gel fraction (%) is calculated as the percentage of the mass of the insoluble pressure-sensitive adhesive sheet remaining in the wire mesh (mass after immersion) relative to the mass of the pressure-sensitive adhesive sheet before immersion in ethyl acetate (mass before immersion).

[0041] Examples of methods for adjusting the gel fraction within the above range include, but are not limited to, a method of adjusting the composition or molecular weight of the acrylic polymer (A) or the type or content of the crosslinking agent (B) or the photoinitiator (C), and a method of adjusting the amount of active energy ray irradiation.

[0042] It is preferable that the present pressure-sensitive adhesive sheet further satisfies the following requirement (7): Requirement (7) The adhesive strength of the acrylic pressure-sensitive adhesive layer to soda-lime glass at a temperature of 23° C. and a peeling rate of 60 mm / min is 2 N / cm or more.

[0043] A pressure-sensitive adhesive sheet that satisfies requirement (7) tends to avoid peeling at the edge of the pressure-sensitive adhesive sheet and to obtain excellent bonding reliability at the peripheral edge. From this viewpoint, the adhesive strength is preferably 2 N / cm or more, more preferably 4 N / cm or more, even more preferably 6 N / cm or more, and particularly preferably 10 N / cm or more. The upper limit of the adhesive strength is usually 50 N / cm, preferably 30 N / cm.

[0044] The adhesive strength is measured, for example, as follows. A 100 μm-thick polyethylene terephthalate (PET) film serving as a backing film is laminated to the acrylic adhesive layer of the adhesive sheet, and the other surface is roll-pressed onto soda-lime glass to obtain a laminate. The laminate is then autoclaved (temperature 60°C, gauge pressure 0.2 MPa, 20 minutes) to obtain a finished laminated product for adhesive strength measurement. This sample is used to peel the adhesive sheet at a peel angle of 180° and a peel rate of 60 mm / min under an environment of 23°C and 50% RH, and the peel force (N / cm) obtained when peeled is taken as the adhesive strength.

[0045] It is preferable that the present pressure-sensitive adhesive sheet further satisfies the following requirement (8): Requirement (8) When the pressure-sensitive adhesive sheet is pressure-bonded to an adherend, the average distance by which the adhesive protrudes from each side of the pressure-sensitive adhesive sheet is 200 μm or less.

[0046] A pressure-sensitive adhesive sheet that satisfies requirement (8) tends to have a low tendency for the edge surface to be crushed during pressure bonding, and to have excellent bonding reliability at the peripheral edge. From this viewpoint, the distance by which the adhesive overflows is preferably 150 μm or less, more preferably 100 μm or less, and even more preferably 80 μm or less. Note that the distance by which the adhesive overflows is usually 0 μm, that is, it is preferable that the adhesive does not overflow.

[0047] The adhesive overflow distance is measured, for example, as follows: After cutting the adhesive sheet into 10 mm x 10 mm pieces, soda lime glass is pressed onto the sheet using a vacuum laminator at a temperature of 23°C, a gauge pressure of 0.4 MPa, and a pressing time of 60 seconds. For the center of each side of the adhesive sheet, the distance between the end position before and after pressing is measured, and the average value of the four sides is taken as the adhesive overflow distance (µm).

[0048] <Present Pressure-Sensitive Adhesive Sheet 1> The present pressure-sensitive adhesive sheet 1 has an acrylic pressure-sensitive adhesive layer formed from a pressure-sensitive adhesive composition containing an acrylic polymer (A). Preferably, the pressure-sensitive adhesive composition further contains a crosslinking agent (B) and a photoinitiator (C). Furthermore, the pressure-sensitive adhesive composition may further contain other components in addition to the acrylic polymer (A), the crosslinking agent (B), and the photoinitiator (C). When the pressure-sensitive adhesive composition is active energy ray-curable, the present pressure-sensitive adhesive sheet 1 is typically obtained by curing a pressure-sensitive adhesive composition containing the acrylic polymer (A). Each component contained in the pressure-sensitive adhesive composition will be described in detail below.

[0049] [Acrylic Polymer (A)] Examples of the acrylic polymer (A) include a homopolymer of alkyl(meth)acrylate and a copolymer obtained by polymerizing a monomer component copolymerizable therewith. Among these, it is preferable that the acrylic polymer (A) contains two or more copolymerization components, and at least one of the copolymerization components is an alkyl(meth)acrylate (a1) having an alkyl group with 3 to 30 carbon atoms (hereinafter, sometimes referred to as "alkyl(meth)acrylate (a1)").

[0050] A more specific example of the acrylic polymer (A) is a copolymer of copolymerization components containing an alkyl(meth)acrylate (a1) and at least one copolymerizable monomer selected from the group consisting of alkyl(meth)acrylate (a1), a hydroxyl group-containing monomer (a2), a nitrogen-containing monomer (a3), a carboxy group-containing monomer (a4), an epoxy group-containing monomer (a5), a vinyl monomer (a6), an alkyl(meth)acrylate monomer (a7) having an alkyl group with 1 or 2 carbon atoms, an alicyclic monomer (a8), a macromonomer (a9), and other copolymerizable monomers (a10) [hereinafter, these may be referred to as "copolymerizable monomers (a2) to (a10)"]. Among these, the inclusion of a hydroxyl group-containing monomer (a2) and / or a nitrogen-containing monomer (a3) ​​as the copolymerization component is preferred in that it enables the combination of corrosion resistance, adhesiveness, and resistance to wet heat whitening when the adherend contains a corrosive component such as a metal, and the inclusion of a hydroxyl group-containing monomer (a2) and a nitrogen-containing monomer (a3) ​​is particularly preferred in that it further enhances cohesion. Furthermore, when the adherend contains a corrosive component such as a metal, it is preferable that the copolymerization component does not contain a carboxyl group-containing monomer (a4) in terms of corrosion resistance. Such an acrylic polymer (A) typically has structural units derived from the alkyl (meth)acrylate (a1) having an alkyl group of 3 to 30 carbon atoms, as well as structural units derived from the copolymerizable monomers (a2) to (a10) contained in the copolymerization component.

[0051] [Alkyl (meth)acrylate (a1)] The alkyl (meth)acrylate (a1) is a linear or branched alkyl (meth)acrylate having an alkyl group with 3 to 30 carbon atoms, and is represented by the following formula (Chemical Formula 1): CH═C(R 1 )-COO(R 2 )...(Chemical formula 1) (In Chemical formula 1, R 1 represents a hydrogen atom or a methyl group, R 2 represents a linear or branched alkyl group having 3 to 30 carbon atoms.

[0052] Examples of the alkyl(meth)acrylate represented by the formula (Chemical Formula 1) include linear alkyl(meth)acrylates such as n-propyl(meth)acrylate, i-propyl(meth)acrylate, n-butyl(meth)acrylate, n-pentyl(meth)acrylate, n-hexyl(meth)acrylate, n-heptyl(meth)acrylate, n-octyl(meth)acrylate, n-nonyl(meth)acrylate, n-decyl(meth)acrylate, undecyl(meth)acrylate, lauryl(meth)acrylate, n-tridecyl(meth)acrylate, n-tetradecyl(meth)acrylate, cetyl(meth)acrylate, stearyl(meth)acrylate, icosyl(meth)acrylate, henicosyl(meth)acrylate, and behenyl(meth)acrylate; sec-butyl(meth)acrylate; Examples of branched alkyl (meth)acrylates include isobutyl (meth)acrylate, t-butyl (meth)acrylate, isopentyl (meth)acrylate, neopentyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, isodecyl (meth)acrylate, isobornyl (meth)acrylate, isostearyl (meth)acrylate, isoicosyl (meth)acrylate, butyloctyl (meth)acrylate, isomyristyl (meth)acrylate, isocetyl (meth)acrylate, hexyldecyl (meth)acrylate, isostearyl (meth)acrylate, octyldecyl (meth)acrylate, octyldodecyl (meth)acrylate, and isobehenyl (meth)acrylate. These may be used alone or in combination of two or more.

[0053] Among these, linear alkyl (meth)acrylates are preferred from the viewpoint of obtaining flexibility. Furthermore, from the viewpoint of balancing adhesiveness and flexibility, linear alkyl (meth)acrylates having an alkyl group of 3 to 20 carbon atoms, more preferably 5 to 18, particularly 6 to 16, and even more particularly 7 to 14 carbon atoms are preferred, and examples thereof include n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, decyl (meth)acrylate, and lauryl (meth)acrylate.

[0054] Among these, branched-chain alkyl(meth)acrylates, i.e., alkyl(meth)acrylates containing a tertiary carbon atom in the alkyl group, are preferred because they facilitate the hydrogen abstraction reaction described below upon irradiation with active energy rays, thereby enabling efficient formation of a crosslinked structure. Among these, branched-chain alkyl(meth)acrylates in which the alkyl group contains 3 to 20 carbon atoms, more preferably 5 to 18, particularly 6 to 16, and even more preferably 7 to 14 carbon atoms, are preferred. For example, sec-butyl(meth)acrylate, isobutyl(meth)acrylate, t-butyl(meth)acrylate, isopentyl(meth)acrylate, neopentyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, isooctyl(meth)acrylate, isononyl(meth)acrylate, isodecyl(meth)acrylate, and isobornyl(meth)acrylate are preferred, with 2-ethylhexyl(meth)acrylate and isobornyl(meth)acrylate being particularly preferred.

[0055] The proportion of the alkyl (meth)acrylate (a1)-derived structural units relative to the acrylic polymer (A) is typically 5 to 95% by mass, preferably 10 to 90% by mass, more preferably 15 to 85% by mass, and particularly preferably 20 to 80% by mass. When the proportion of the alkyl (meth)acrylate (a1)-derived structural units is equal to or greater than the lower limit, the composition tends to have excellent flexibility and excellent conformability to uneven surfaces of the adherend. When the proportion is equal to or less than the upper limit, the effect of the copolymerizable monomer described below is easily obtained, and the composition tends to have excellent adhesive strength and cohesive strength.

[0056] [Hydroxyl Group-Containing Monomer (a2)] Examples of the hydroxyl group-containing monomer (a2) include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 5-hydroxypentyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and 8-hydroxyoctyl (meth)acrylate; caprolactone-modified hydroxy (meth)acrylates such as caprolactone-modified 2-hydroxyethyl (meth)acrylate; diethylene glycol (meth)acrylate; polyethylene glycol (meth)acrylate; polypropylene glycol (meth)acrylate; polytetramethylene glycol (meth)acrylate; polyoxyethylene poly(meth)acrylate; Examples of such monomers include (meth)acrylates having an oxyalkylene structure such as propylene glycol (meth)acrylate, primary hydroxyl group-containing (meth)acrylates such as 2-acryloyloxyethyl-2-hydroxyethyl phthalate, secondary hydroxyl group-containing (meth)acrylates such as 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, and 3-chloro-2-hydroxypropyl (meth)acrylate, tertiary hydroxyl group-containing (meth)acrylates such as 2,2-dimethyl 2-hydroxyethyl (meth)acrylate, and vinyl ethers such as 2-hydroxyethyl vinyl ether, diethylene glycol monovinyl ether, and 4-hydroxybutyl vinyl ether. These may be used alone or in combination of two or more. The hydroxyl group-containing monomer (a2) improves the adhesive strength of the pressure-sensitive adhesive sheet and can suppress whitening under heat and humidity. Furthermore, when the pressure-sensitive adhesive composition contains a thermal crosslinking agent, as described below, it serves as a crosslinking reaction site.

[0057] Among the hydroxyl group-containing monomers (a2), preferred are hydroxyl group-containing monomers having a hydroxyalkyl group having 1 to 10, more preferably 1 to 6, and even more preferably 2 to 4 carbon atoms, such as 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxyethyl vinyl ether, diethylene glycol monovinyl ether, and 4-hydroxybutyl vinyl ether, and particularly preferred are primary hydroxyl group-containing (meth)acrylates, such as 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate.

[0058] When the acrylic polymer (A) has a structural unit derived from a hydroxyl group-containing monomer (a2), the content thereof is usually 3 to 30% by mass, preferably 5 to 25% by mass, and particularly preferably 7 to 20% by mass, based on the acrylic polymer (A), from the viewpoint of imparting adhesive strength and resistance to wet heat whitening.

[0059] [Nitrogen-Containing Monomer (a3)] Examples of the nitrogen-containing monomer (a3) ​​include amino group-containing monomers, amide group-containing monomers, isocyanate group-containing monomers, and (meth)acrylonitrile. These may be used alone or in combination of two or more. The nitrogen-containing monomer (a3) ​​improves the cohesive strength of the pressure-sensitive adhesive sheet and can suppress wet heat whitening. Furthermore, when a hydrogen abstraction photoinitiator described below is used, it is preferable that the acrylic polymer (A) has a structural unit derived from the nitrogen-containing monomer (a3). When a hydrogen abstraction photoinitiator described below is used, the nitrogen-containing monomer (a3) ​​has the effect of promoting the hydrogen abstraction reaction.

[0060] Examples of the amino group-containing monomer include primary amino group-containing (meth)acrylates such as aminomethyl (meth)acrylate and aminoethyl (meth)acrylate; secondary amino group-containing (meth)acrylates such as t-butylaminoethyl (meth)acrylate and t-butylaminopropyl (meth)acrylate; tertiary amino group-containing (meth)acrylates such as ethylaminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, diethylaminopropyl (meth)acrylate, and dimethylaminopropylacrylamide; and monomers such as N-vinylpyrrolidone, methylvinylpyrrolidone, vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole, vinylmorpholine, (meth)acryloylmorpholine, N-vinylacetamides, and N-vinylcaprolactam.

[0061] Examples of the amide group-containing monomer include (meth)acrylamide; N-alkyl(meth)acrylamides such as N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N-propyl(meth)acrylamide, N-n-butyl(meth)acrylamide, diacetone(meth)acrylamide, and N,N'-methylenebis(meth)acrylamide; N,N-dialkyl(meth)acrylamides such as N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropyl(meth)acrylamide, N,N-ethylmethylacrylamide, and N,N-diallyl(meth)acrylamide; hydroxyalkyl(meth)acrylamides such as N-hydroxymethyl(meth)acrylamide and N-hydroxyethyl(meth)acrylamide; alkoxyalkyl(meth)acrylamides such as N-methoxymethyl(meth)acrylamide and N-(n-butoxymethyl)(meth)acrylamide; maleimide or a derivative thereof. Among these, (meth)acrylamide is preferred.

[0062] Examples of the isocyanate group-containing monomer include 2-(meth)acryloyloxyethyl isocyanate and alkylene oxide adducts thereof, etc. The isocyanate group may be protected with a blocking agent such as methyl ethyl ketone oxime, 3,5-dimethylpyrazole, 1,2,4-triazole, or diethyl malonate.

[0063] Among these, those having a tertiary nitrogen atom are preferred, as they have a sensitizing effect on the hydrogen abstraction reaction by the hydrogen abstraction photoinitiator described below, and as a result, can efficiently form a crosslinked structure. Tertiary amino group-containing (meth)acrylates, N,N-dialkyl(meth)acrylamides, N-vinylpyrrolidone, acryloylmorpholine, and the like are particularly preferred.

[0064] When the acrylic polymer (A) has a structural unit derived from a nitrogen-containing monomer (a3), the content thereof is usually 0.1 to 15 mass%, preferably 0.5 to 13 mass%, particularly preferably 1 to 10 mass%, and especially preferably 2 to 7 mass%, relative to the acrylic polymer (A), from the viewpoint of imparting cohesive strength and resistance to wet heat whitening.

[0065] [Carboxy Group-Containing Monomer (a4)] Examples of the carboxy group-containing monomer (a4) include (meth)acrylic acid, 2-(meth)acryloyloxyethyl hexahydrophthalic acid, 2-(meth)acryloyloxypropyl hexahydrophthalic acid, 2-(meth)acryloyloxyethyl phthalic acid, 2-(meth)acryloyloxypropyl phthalic acid, 2-(meth)acryloyloxyethyl maleic acid, 2-(meth)acryloyloxypropyl maleic acid, 2-(meth)acryloyloxyethyl succinic acid, 2-(meth)acryloyloxypropyl succinic acid, crotonic acid, fumaric acid, maleic acid, itaconic acid, etc. These may be used alone or in combination of two or more.

[0066] When the acrylic polymer (A) has a structural unit derived from a carboxy group-containing monomer (a4), the content thereof is usually 0.1 to 15 mass%, preferably 0.3 to 13 mass%, more preferably 0.5 to 10 mass%, and particularly preferably 1 to 6 mass%, based on the acrylic polymer (A).

[0067] [Epoxy Group-Containing Monomer (a5)] Examples of the epoxy group-containing monomer (a5) include glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate glycidyl ether. These may be used alone or in combination of two or more.

[0068] When the acrylic polymer (A) has a structural unit derived from an epoxy group-containing monomer (a5), the content thereof is usually 0.1 to 15 mass%, preferably 0.3 to 13 mass%, more preferably 0.5 to 10 mass%, and particularly preferably 1 to 6 mass%, based on the acrylic polymer (A).

[0069] [Vinyl Monomer (a6)] Examples of the vinyl monomer (a6) include compounds having a vinyl group in the molecule. Examples of such compounds include vinyl ester monomers such as vinyl acetate, vinyl propionate, vinyl laurate, and vinyl stearate, as well as aromatic vinyl monomers such as styrene, chlorostyrene, chloromethylstyrene, α-methylstyrene, and other substituted styrenes. These may be used alone or in combination of two or more. These may be used alone or in combination of two or more.

[0070] When the acrylic polymer (A) has a constituent moiety derived from a vinyl monomer (a6), the content thereof is, from the viewpoint of imparting cohesive strength to the PSA sheet, usually 1 to 40 mass %, preferably 5 to 35 mass %, more preferably 8 to 30 mass %, and particularly preferably 10 to 25 mass %, relative to the acrylic polymer (A).

[0071] [Alkyl(meth)acrylate Monomer (a7) in Which the Alkyl Group Has 1 or 2 Carbon Atoms] Examples of the alkyl(meth)acrylate monomer (a7) in Which the alkyl group has 1 or 2 carbon atoms include methyl(meth)acrylate and ethyl(meth)acrylate. These may be used alone or in combination of two or more.

[0072] When the acrylic polymer (A) has a structural unit derived from an alkyl(meth)acrylate monomer (a7), the content thereof is, from the viewpoint of imparting cohesive strength to the PSA sheet, usually 1 to 60 mass%, preferably 5 to 55 mass%, particularly preferably 10 to 50 mass%, and especially preferably 15 to 45 mass%, relative to the acrylic polymer (A).

[0073] [Alicyclic Monomer (a8)] Examples of the alicyclic monomer (a8) include cyclohexyl (meth)acrylate, 3,3,5-trimethylcyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, adamantyl (meth)acrylate, etc. These may be used alone or in combination of two or more.

[0074] When the acrylic polymer (A) has a structural unit derived from an alicyclic monomer (a8), the content thereof is, from the viewpoint of imparting cohesive strength to the PSA sheet, usually 0.1 to 15 mass%, preferably 0.5 to 13 mass%, particularly preferably 1 to 10 mass%, and especially preferably 2 to 7 mass%, relative to the acrylic polymer (A).

[0075] [Macromonomer (a9)] The macromonomer (a9) is a monomer that, when polymerized into the acrylic polymer (A), can easily increase the number of carbon atoms in the side chain of the acrylic polymer (A), for example, to 20 or more. By using the macromonomer (a9) as a copolymerization component, the acrylic polymer (A) can be made into a graft copolymer having a constituent portion (segment) derived from the macromonomer (a9). Furthermore, by changing the blending ratio of the macromonomer (a9) to other monomers, the properties of the main chain and side chain of the graft copolymer can be changed.

[0076] The macromonomer (a9) has a radically polymerizable functional group or a functional group such as a hydroxy group, an isocyanate group, an epoxy group, a carboxy group, an amino group, an amide group, or a thiol group. The macromonomer (a9) may have these functional groups alone or in combination of two or more. Among these, the macromonomer (a9) preferably has a radically polymerizable functional group copolymerizable with other monomers. The macromonomer (a9) may contain one or more radically polymerizable functional groups, with one being particularly preferred. Furthermore, when the macromonomer (a9) has a functional group, the macromonomer may contain one or more functional groups, with one being particularly preferred.

[0077] The macromonomer (a9) preferably has a backbone component composed of an acrylic polymer or a vinyl polymer. Examples of backbone components of the macromonomer (a9) include alkyl(meth)acrylates (a1) in which the alkyl group has 3 to 30 carbon atoms, the vinyl monomers (a6), alkyl(meth)acrylate monomers (a7) in which the alkyl group has 1 or 2 carbon atoms, and alicyclic monomers (a8). These may be used alone or in combination of two or more. Among these, the use of alkyl(meth)acrylates or alicyclic monomers in which the alkyl group has 1 to 8 carbon atoms, or aromatic monomers such as styrene, as backbone components is preferred, as they can provide pressure-sensitive adhesive sheets with excellent cohesive strength. On the other hand, the use of alkyl(meth)acrylates in which the alkyl group has 9 to 30 carbon atoms is preferred, as they can provide pressure-sensitive adhesive sheets with excellent flexibility.

[0078] The number average molecular weight of the macromonomer (a9) is preferably from 1,000 to 40,000, more preferably from 1,500 to 20,000, and even more preferably from 2,000 to 15,000. The number average molecular weight of the macromonomer (a9) is a value measured by gel permeation chromatography (GPC) in terms of standard polystyrene.

[0079] As the macromonomer (a9), a generally produced macromonomer (for example, a macromonomer manufactured by Toagosei Co., Ltd.) can be used appropriately.

[0080] When the acrylic polymer (A) has a structural unit derived from macromonomer (a9), the content thereof is usually 1 to 30% by mass, preferably 3 to 20% by mass, and more preferably 5 to 18% by mass, relative to the acrylic polymer (A). If the content is equal to or greater than the lower limit, the phase separation force between the segment containing the structural unit derived from macromonomer (a9) and the segment formed by the other structural units becomes stronger, and the cohesive strength of the PSA sheet tends to be better. If the content is equal to or less than the upper limit, the phase-separated structure tends to collapse more easily during lamination, and the unevenness-following ability tends to be better.

[0081] [Other Copolymerizable Monomers (a10)] Examples of the other copolymerizable monomers (a10) include (meth)acrylates having an alkoxyalkylene glycol skeleton, such as methoxydiethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, butoxypolyethylene glycol (meth)acrylate, methoxypolypropylene glycol (meth)acrylate, butoxypolypropylene glycol (meth)acrylate, methoxypolytetramethylene glycol (meth)acrylate, butoxypolytetramethylene glycol (meth)acrylate, methoxypolyoxyethylene polyoxypropylene glycol (meth)acrylate, and butoxypolyoxyethylene polyoxypropylene glycol (meth)acrylate; phenyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenyldiethylene glycol (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, and phenoxypolyethylene glycol-polypropylene glycol-(meth)acrylate; aromatic (meth)acrylates such as acrylate and nonylphenol ethylene oxide adduct (meth)acrylate, 4-acryloyloxybenzophenone, 4-acryloyloxyethoxybenzophenone, 4-acryloyloxy-4'-methoxybenzophenone, 4-acryloyloxyethoxy-4'-methoxybenzophenone, 4-acryloyloxy-4'-bromobenzophenone, 4-acryloyloxyethoxy-4'-bromobenzophenone, 4-methacryloyloxybenzophenone, 4- Examples include (meth)acrylates having a benzophenone structure such as methacryloyloxyethoxybenzophenone, 4-methacryloyloxy-4'-methoxybenzophenone, 4-methacryloyloxyethoxy-4'-methoxybenzophenone, 4-methacryloyloxy-4'-bromobenzophenone, 4-methacryloyloxyethoxy-4'-bromobenzophenone, and mixtures thereof, heterocycle-containing (meth)acrylates such as tetrahydrofurfuryl (meth)acrylate, and macromonomers. These may be used alone or in combination of two or more.

[0082] When the acrylic polymer (A) has a structural unit derived from another copolymerizable monomer (a10), the content thereof is usually 1 to 30% by mass, preferably 3 to 20% by mass, and more preferably 5 to 15% by mass, based on the acrylic polymer (A).

[0083] The method for producing the acrylic polymer (A) is not particularly limited, and may be, for example, by polymerizing a copolymerization component containing an alkyl(meth)acrylate (a1) and, if necessary, at least one selected from the group consisting of copolymerizable monomers (a2) to (a10).

[0084] Examples of the polymerization method include conventionally known methods such as solution polymerization, suspension polymerization, bulk polymerization, and emulsion polymerization. Among these, solution polymerization is preferred in that it allows safe and stable production of an acrylic resin with any monomer composition. Thus, the acrylic polymer (A) can be obtained.

[0085] The acrylic polymer (A) may have a photoactive moiety, such as a polymerizable carbon-carbon double bond group, introduced into its side chain, thereby enhancing the crosslinking efficiency of the pressure-sensitive adhesive composition and enabling the pressure-sensitive adhesive composition to be crosslinked in a shorter time, thereby increasing productivity.

[0086] Examples of a method for introducing a polymerizable carbon-carbon double bond group into the side chain of the acrylic polymer (A) include a method in which a copolymer containing a functional group-containing ethylenically unsaturated monomer such as the above-mentioned hydroxyl group-containing monomer (a2), nitrogen atom-containing monomer (a3), carboxy group-containing monomer (a4), or epoxy group-containing monomer (a5) is prepared, and then a compound having a polymerizable carbon-carbon double bond group and a functional group reactive with the functional group is subjected to a condensation or addition reaction while maintaining the activity of the polymerizable carbon-carbon double bond group.

[0087] Examples of combinations of these functional groups include an epoxy group (glycidyl group) and a carboxy group, an amino group and a carboxy group, an amino group and an isocyanate group, an epoxy group (glycidyl group) and an amino group, a hydroxyl group and an epoxy group, and a hydroxyl group and an isocyanate group. Among these combinations of functional groups, a combination of a hydroxyl group and an isocyanate group is preferred because of the ease of reaction control. Among these, a combination in which the copolymer has a hydroxyl group and the compound has an isocyanate group is preferred.

[0088] Examples of the isocyanate compound having a polymerizable carbon-carbon double bond group include the above-mentioned 2-(meth)acryloyloxyethyl isocyanate and alkylene oxide adducts thereof.

[0089] From the viewpoint of improving adhesiveness and stress relaxation properties, the content of the compound having a functional group reactive with the functional group and a polymerizable carbon-carbon double bond group is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, even more preferably 1 part by mass or less, and particularly preferably 0.1 parts by mass or less, relative to 100 parts by mass of the acrylic polymer (A). The lower limit is usually 0 part by mass.

[0090] The weight average molecular weight (Mw) of the acrylic polymer (A) is preferably 200,000 or more, more preferably 300,000 or more, and even more preferably 400,000 or more, from the viewpoint of obtaining a pressure-sensitive adhesive composition with high cohesive strength. Furthermore, the upper limit of the weight average molecular weight (Mw) of the acrylic polymer (A) is preferably 1.5 million or less, more preferably 1.2 million or less, even more preferably 1.1 million or less, and particularly preferably 1 million or less, from the viewpoint of ease of handling and uniform stirring. The lower and upper limits of the weight average molecular weight of the acrylic polymer (A) can be arbitrarily combined. The weight average molecular weight of the acrylic polymer (A) is a value calculated in terms of standard polystyrene measured by gel permeation chromatography (GPC).

[0091] The acrylic polymer (A) is preferably the main component of the pressure-sensitive adhesive composition. Here, "main component" refers to the component with the highest content among the components of the pressure-sensitive adhesive composition. Specifically, the content of the acrylic polymer (A) is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more, based on the total mass of the pressure-sensitive adhesive composition. The upper limit is 100% by mass, but is usually preferably 99% by mass or less, more preferably 98% by mass or less, and even more preferably 97% by mass or less.

[0092] [Crosslinking Agent (B)] The pressure-sensitive adhesive composition preferably contains a crosslinking agent (B) from the viewpoint of promoting the crosslinking reaction. This allows the pressure-sensitive adhesive composition to efficiently form a crosslinked structure. Furthermore, when a crosslinked structure is formed in a pressure-sensitive adhesive sheet using the pressure-sensitive adhesive composition, adhesive extrusion during storage or application can be prevented, and good adhesiveness and cohesive strength can be obtained. However, when the acrylic polymer (A) undergoes a hydrogen abstraction reaction due to the action of a photoinitiator (C) described below or the like, and a sufficient crosslinked structure can be formed within the acrylic polymer (A) and / or between the acrylic polymers (A), the crosslinking agent (B) does not necessarily need to be contained.

[0093] Examples of the crosslinking agent (B) include acrylic crosslinking agents, isocyanate crosslinking agents, epoxy crosslinking agents, aziridine crosslinking agents, melamine crosslinking agents, aldehyde crosslinking agents, amine crosslinking agents, and metal chelate crosslinking agents. These may be used alone or in combination of two or more. Among these, isocyanate crosslinking agents are preferred because of their excellent reactivity with the acrylic polymer (A). On the other hand, acrylic crosslinking agents are preferred, and polyfunctional (meth)acrylates are particularly preferred, from the viewpoints of ease of reaction control and active energy ray curability.

[0094] Examples of the polyfunctional (meth)acrylate include polyfunctional (meth)acrylic monomers and polyfunctional (meth)acrylic oligomers having two or more (meth)acryloyl groups, which may be used alone or in combination of two or more.

[0095] Examples of the polyfunctional (meth)acrylic monomer include pentanediol di(meth)acrylate, hexadiol di(meth)acrylate, heptanediol di(meth)acrylate, octanediol di(meth)acrylate, nonanediol di(meth)acrylate, decanediol di(meth)acrylate, undecanediol di(meth)acrylate, dodecanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, glycerin di(meth)acrylate, neopentyl glycol di(meth)acrylate, glycerin glycidyl ether di(meth)acrylate, tricyclodecane dimethacrylate, tricyclodecane dimethanol di(meth)acrylate, bisphenol A polyethoxy di(meth)acrylate, bisphenol A polypropoxy di(meth)acrylate, bisphenol F polyethoxy di(meth)acrylate, ethylene glycol di(meth)acrylate tri(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane trioxyethyl (meth)acrylate, ε-caprolactone-modified tris(2-hydroxyethyl) isocyanurate tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propoxylated pentaerythritol tri(meth)acrylate, ethoxylated pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, propoxylated pentaerythritol tri(meth)acrylate Pentaerythritol tetra(meth)acrylate, ethoxylated pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, tris(acryloxyethyl)isocyanurate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol penta(meth)acrylate , tripentaerythritol hexa(meth)acrylate, tripentaerythritol penta(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, di(meth)acrylate of hydroxypivalic acid neopentyl glycol ε-caprolactone adduct, trimethylolpropane tri(meth)acrylate, trimethylolpropane polyethoxytri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, etc.

[0096] Examples of the polyfunctional (meth)acrylic oligomer include polyester (meth)acrylate oligomers, epoxy (meth)acrylate oligomers, urethane (meth)acrylate oligomers, and polyether (meth)acrylate oligomers.

[0097] Among these crosslinking agents (B), polyfunctional (meth)acrylate monomers and oligomers having a glycol structure are preferred from the viewpoint of imparting appropriate flexibility to the cured product, and acrylic acid adducts of pentaerythritol and dipentaerythritol, and alkoxylated products thereof are preferred from the viewpoint of imparting cohesive strength.

[0098] When the pressure-sensitive adhesive composition contains a crosslinking agent (B), the content thereof is usually 0.1 parts by mass or more, preferably 0.5 parts by mass or more, and more preferably 1 part by mass or more, per 100 parts by mass of the acrylic polymer (A), from the viewpoint of imparting shape stability to the pressure-sensitive adhesive sheet and durability when formed into a laminate for an image display device. Furthermore, the upper limit is usually 25 parts by mass or less, preferably 22 parts by mass or less, more preferably 20 parts by mass or less, and particularly preferably 18 parts by mass or less, from the viewpoint of maintaining the flexibility of the pressure-sensitive adhesive sheet. The lower and upper limits of the content of the crosslinking agent (B) can be arbitrarily combined.

[0099] [Photoinitiator (C)] The pressure-sensitive adhesive composition preferably contains a photoinitiator (C). The photoinitiator (C) is a compound that generates radicals when exposed to active energy rays. The photoinitiators (C) are broadly classified into two types based on the radical generation mechanism. More specifically, they are broadly classified into cleavage-type photoinitiators, which can generate radicals by cleaving and decomposing the single bond of the photoinitiator itself, and hydrogen-abstraction-type photoinitiators, which can generate radicals by the excited initiator abstracting hydrogen from a hydrogen donor in the system. These may be used alone or in combination of two or more types. The cleavage-type photoinitiator is preferred because it has high photosensitivity. On the other hand, the hydrogen-abstraction-type photoinitiator is preferred because it does not generate photodecomposition products and can incorporate the acrylic polymer (A) into a crosslinked structure through a hydrogen abstraction reaction.

[0100] Examples of the hydrogen abstraction photoinitiator include benzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, 4-phenylbenzophenone, 3,3'-dimethyl-4-methoxybenzophenone, methyl 2-benzoylbenzoate, 4-[(4-methylphenyl)thio]benzophenone, 4-acryloyloxybenzophenone, 4-acryloyloxyethoxybenzophenone, 4-acryloyloxy-4'-methoxybenzophenone, 4-acryloyloxyethoxy-4'-methoxybenzophenone, 4-acryloyloxy-4'-bromobenzophenone, 4-acryloyloxyethoxy-4'-bromobenzophenone, 4-methacryloyloxy-4'-bromobenzophenone, Examples of suitable photoinitiators include intermolecular hydrogen abstraction photoinitiators such as acryloyloxybenzophenone, 4-methacryloyloxyethoxybenzophenone, 4-methacryloyloxy-4'-methoxybenzophenone, 4-methacryloyloxyethoxy-4'-methoxybenzophenone, 4-methacryloyloxy-4'-bromobenzophenone, and 4-methacryloyloxyethoxy-4'-bromobenzophenone; and intramolecular hydrogen abstraction photoinitiators such as methylbenzoyl formate, methyl benzoylformate, oxyphenylacetic acid-2-(2-oxo-2-phenyl-acetoxy-ethoxy)ethyl ester, and oxyphenylacetic acid-2-(2-hydroxy-ethoxy)ethyl ester. These may be used alone or in combination of two or more.

[0101] Among the intermolecular hydrogen abstraction photoinitiators, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, and photoinitiators (c1) having a radically polymerizable functional group having a carbon-carbon double bond and a structure that generates radicals in the molecule, such as 4-acryloyloxybenzophenone, 4-methacryloyloxybenzophenone, 4-acryloyloxyethoxybenzophenone, 4-acryloyloxy-4'-methoxybenzophenone, 4-acryloyloxyethoxy-4'-methoxybenzophenone, and 4-methacryloyloxybenzophenone are preferred, and 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, 4-methacryloyloxybenzophenone, and 4-methacryloyloxybenzophenone are more preferred. The photoinitiator (c1) having a radical-polymerizable functional group having a carbon-carbon double bond and a structure that generates radicals in its molecule is incorporated into the polymerization structure after photoreaction, which tends to suppress bleed-out of the photoinitiator and improve the cohesive strength of the PSA sheet. Furthermore, intramolecular hydrogen abstraction photoinitiators are preferred because they can act not only as hydrogen donors in the system but also as starting points for radical generation, with methylbenzoyl formate being more preferred.

[0102] Examples of the cleavage-type photoinitiator include 2,2-dimethoxy-1,2-diphenylethan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)benzyl]phenyl}-2-methyl-propan-1-one, oligo(2-hydroxy-2-methyl-1-(4-(1-methylvinyl)phenyl)propanone), 2-benzyl-2-dimethylamino-1-(4-morpholino)-1-propanone, ... Examples of the methyl benzoyl ester include 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, (2,4,6-trimethylbenzoyl)ethoxyphenylphosphine oxide, bis(2,6-dimethoxybenzoyl)2,4,4-trimethylpentylphosphine oxide, and derivatives thereof. These may be used alone or in combination of two or more.

[0103] In the present invention, it is preferable that the photoinitiator (C) contains an intermolecular hydrogen abstraction photoinitiator and an intramolecular hydrogen abstraction photoinitiator, from the viewpoint of increasing the cohesive strength of the pressure-sensitive adhesive sheet.

[0104] Furthermore, in the present invention, the photoinitiator (C) preferably includes a photoinitiator (c1) having a radically polymerizable functional group having a carbon-carbon double bond and a structure that generates radicals in its molecule, and a hydrogen abstraction photoinitiator (c2) other than the photoinitiator (c1). The combined use of these photoinitiators (C) can enhance the cohesive strength of the pressure-sensitive adhesive sheet. Furthermore, when the pressure-sensitive adhesive sheet is active energy ray-curable, it can be a pressure-sensitive adhesive sheet that exhibits excellent secondary curing properties after being attached to an adherend. The hydrogen abstraction photoinitiator (c2) refers to a hydrogen abstraction photoinitiator other than the photoinitiator (c1) having a radically polymerizable functional group having a carbon-carbon double bond and a structure that generates radicals in its molecule. Among the hydrogen abstraction photoinitiators (c2), intramolecular hydrogen abstraction photoinitiators are preferred because they can act not only as hydrogen donors in the system but also as initiators of radical generation themselves, with methylbenzoyl formate being more preferred.

[0105] When the pressure-sensitive adhesive composition contains a photoinitiator (C), the content thereof is usually 10 parts by mass or less, preferably 5 parts by mass or less, more preferably 4 parts by mass or less, and particularly preferably 3 parts by mass or less, relative to 100 parts by mass of the acrylic polymer (A). The lower limit is usually 0.1 parts by mass. When two or more types of photoinitiators (C) are used in combination, the above content is the total amount of the photoinitiators (C) used.

[0106] When the photoinitiator (C) contains a photoinitiator (c1) having, in the molecule, a radical-polymerizable functional group having a carbon-carbon double bond and a structure that generates a radical, and a hydrogen abstraction photoinitiator (c2) other than the photoinitiator (c1), the mass ratio (c2 / c1) of the photoinitiator (c2) to the photoinitiator (c1) is preferably 0.5 to 10, more preferably 1 to 8, and even more preferably 2 to 6.

[0107] [Monofunctional (meth)acrylate] The pressure-sensitive adhesive composition may further contain a monofunctional (meth)acrylate having one (meth)acryloyl group, if necessary. By containing a monofunctional (meth)acrylate having one (meth)acryloyl group, the molecular weight between crosslinking points of the cured product can be increased, which increases the degree of freedom of movement of the molecular chain and makes it easier to obtain appropriate stress relaxation properties.

[0108] Examples of the monofunctional (meth)acrylate include ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, amyl (meth)acrylate, isoamyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, and dodecyl (meth)acrylate. (meth)acrylate, isododecyl (meth)acrylate, tetradecyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, behenyl (meth)acrylate, cyclopropyl (meth)acrylate, cyclobutyl (meth)acrylate, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, cycloheptyl (meth)acrylate, cyclooctyl (meth)acrylate, cyclononyl (meth)acrylate, cyclodecyl (meth)acrylate, isobornyl (meth)acrylate acrylate, norbornyl (meth)acrylate, adamantyl (meth)acrylate, tricyclodecane dimethanol acrylate, ethoxylated-o-phenylphenol acrylate, 2-hydroxy-o-phenylphenol propyl acrylate, methoxypolyethylene glycol (meth)acrylate, methoxypolypropylene glycol (meth)acrylate, polyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, phenoxyethylene glycol (meth)acrylate, phenoxydiethylene glycol benzyl (meth)acrylates such as chol (meth)acrylate, phenoxy polyethylene glycol (meth)acrylate, 2-hydroxy-o-phenylphenol propyl acrylate, 2-(meth)acryloyloxyethyl succinate, 2-(meth)acryloyloxyethyl tetrahydrophthalate, 2-(meth)acryloyloxyethyl hexahydrophthalate, 2-(meth)acryloyloxypropyl phthalate, 2-(meth)acryloyloxypropyl hydrophthalate, and 2-(meth)acryloyloxypropyl hexahydrophthalate;Benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxyethylene glycol (meth)acrylate, 2-naphthyl (meth)acrylate, 9-anthracenyl (meth)acrylate, 1-pyrenylmethyl (meth)acrylate, benzyl (meth)acrylate, tricyclodecane dimethanol monoacrylate monocarboxylic acid, dicyclopentanyl acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, trimethylolpropane mono(meth)acrylate, glycerin mono(meth)acrylate, pentaerythritol mono(meth)acrylate, diglycerin mono(meth)acrylate, ditrimethylolpropane mono(meth)acrylate, di Examples include pentaerythritol mono(meth)acrylate, ethoxylated trimethylolpropane mono(meth)acrylate, propoxylated trimethylolpropane mono(meth)acrylate, ethoxylated glycerin mono(meth)acrylate, propoxylated glycerin mono(meth)acrylate, ethoxylated pentaerythritol mono(meth)acrylate, propoxylated pentaerythritol mono(meth)acrylate, ethoxylated ditrimethylolpropane mono(meth)acrylate, propoxylated ditrimethylolpropane mono(meth)acrylate, alkylene oxide-modified diglycerin mono(meth)acrylate, and alkylene oxide-modified dipentaerythritol mono(meth)acrylate, as well as monofunctional oligomers such as monofunctional urethane (meth)acrylate, monofunctional epoxy (meth)acrylate, and monofunctional polyester (meth)acrylate. These may be used alone or in combination of two or more.

[0109] When the monofunctional (meth)acrylate component is contained, the content thereof is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and particularly preferably 5 parts by mass or more, per 100 parts by mass of the acrylic polymer (A), from the viewpoint of adjusting the crosslinking density and imparting appropriate flexibility to the cured product. The upper limit is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, and particularly preferably 5 parts by mass or less.

[0110] [Other Components] The pressure-sensitive adhesive composition may contain, as needed, various additives such as silane coupling agents, ultraviolet absorbers, plasticizers, tackifiers, antioxidants, light stabilizers, metal deactivators, anti-aging agents, moisture absorbers, rust inhibitors, and inorganic particles as "other components" as long as the effects of the present invention are not impaired. Furthermore, the pressure-sensitive adhesive composition may contain, as needed, reaction catalysts such as tertiary amine compounds, quaternary ammonium compounds, and tin laurate compounds. These may be used alone or in combination of two or more. These may be used alone or in combination of two or more. It is particularly preferred that the pressure-sensitive adhesive composition contain a silane coupling agent.

[0111] [Silane coupling agent] The silane coupling agent is an organosilicon compound that contains one or more reactive functional groups and one or more alkoxy groups bonded to silicon atoms in its structure.The reactive functional groups include, for example, epoxy group, (meth)acryloyl group, mercapto group, hydroxyl group, carboxy group, amino group, amide group, and isocyanate group.Among these, epoxy group and mercapto group are preferred from the viewpoint of balance of durability.

[0112] The alkoxy group bonded to the silicon atom preferably contains an alkoxy group having 1 to 8 carbon atoms, from the viewpoint of durability and storage stability, and is particularly preferably a methoxy group or an ethoxy group. The silane coupling agent may also contain an organic substituent other than the reactive functional group and the alkoxy group bonded to the silicon atom, such as an alkyl group or a phenyl group.

[0113] Examples of the silane coupling agent include monomeric epoxy group-containing silane coupling agents, which are silane compounds such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; and silane coupling agents in which a part of the silane compound is hydrolyzed and condensed, or in which the silane compound is polymerized with methyltriethoxysilane, ethyltriethoxysilane, oligomeric epoxy group-containing silane coupling agents which are silane compounds obtained by co-condensation of alkyl group-containing silane compounds such as methyltrimethoxysilane and ethyltrimethoxysilane; monomeric mercapto group-containing silane coupling agents which are silane compounds such as 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, γ-mercaptopropyldimethoxymethylsilane and 3-mercaptopropylmethyldimethoxysilane; and silane coupling agents which are obtained by hydrolysis and condensation polymerization of a part of the silane compounds or by condensation polymerization of the silane compounds with methyl groups. oligomeric mercapto group-containing silane coupling agents which are silane compounds obtained by co-condensation of alkyl group-containing silane compounds such as 3-acryloxypropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane; (meth)acryloyl group-containing silane coupling agents such as 3-acryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane; coupling agents: amino group-containing silane coupling agents such as N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, and N-phenyl-3-aminopropyltrimethoxysilane; isocyanate group-containing silane coupling agents such as 3-isocyanatepropyltriethoxysilane;Examples of suitable silane coupling agents include vinyl group-containing silane coupling agents such as vinyltrimethoxysilane and vinyltriethoxysilane. These may be used alone or in combination of two or more.

[0114] Among these, epoxy group-containing silane coupling agents and mercapto group-containing silane coupling agents are preferably used because of their excellent durability, and among these, epoxy group-containing silane coupling agents are particularly preferred.

[0115] When the pressure-sensitive adhesive composition contains a silane coupling agent, the content thereof is usually 0.005 to 10 parts by mass, preferably 0.01 to 5 parts by mass, and particularly preferably 0.05 to 1 part by mass, relative to 100 parts by mass of the acrylic polymer (A). When the content is within the above range, adhesive strength and durability tend to be improved.

[0116] [Plasticizer] The plasticizer may be, but is not limited to, at least one selected from the group consisting of polyisobutylene, polyisoprene, polybutadiene, amorphous polyolefins and their copolymers, silicone, polyacrylate, oligomeric polyurethane, ethylene-propylene copolymer, etc., or any combination or mixture thereof. Among these, polyisobutylene is preferred. The polyisobutylene plasticizer may be, for example, one selected from the OPPANOLB series, which is commercially available from BASF under the trade name OPPANOL.

[0117] When the pressure-sensitive adhesive composition contains a plasticizer, the content thereof is not particularly limited and is usually 0.1 to 20 parts by mass, preferably 0.5 to 15 parts by mass, per 100 parts by mass of the acrylic polymer (A).

[0118] [Tackifier] The PSA composition may contain a tackifier to improve the adhesive strength of the PSA sheet. Examples of the tackifier include terpene resins such as polyterpenes (e.g., α-pinene resins, β-pinene resins, and limonene resins) and aromatic-modified polyterpene resins (e.g., phenol-modified polyterpene resins), coumaran-indene resins, petroleum-based resins such as C5 hydrocarbon resins, C9 hydrocarbon resins, C5 / C9 hydrocarbon resins, and dicyclopentadiene resins, and rosins such as modified rosin, hydrogenated rosin, polymerized rosin, and rosin ester. These may be used alone or in combination of two or more.

[0119] When the pressure-sensitive adhesive composition contains a tackifier, the content thereof is not particularly limited and is usually 0.1 to 20 parts by mass, preferably 0.5 to 15 parts by mass, per 100 parts by mass of the acrylic polymer (A).

[0120] [Rust inhibitor] The pressure-sensitive adhesive composition may contain a rust inhibitor to prevent corrosion when the adherend includes a corrosive portion such as metal wiring. Examples of the rust inhibitor include triazoles and benzotriazoles. These may be used alone or in combination of two or more.

[0121] The content of the rust inhibitor in the pressure-sensitive adhesive composition is usually 0.01 to 5 parts by mass, and preferably 0.1 to 3 parts by mass, per 100 parts by mass of the acrylic polymer (A).

[0122] <Method for manufacturing the present pressure-sensitive adhesive sheet 1> Next, a description will be given of a method for manufacturing the present pressure-sensitive adhesive sheet 1. However, the following description is an example of a method for manufacturing the present pressure-sensitive adhesive sheet 1, and the present pressure-sensitive adhesive sheet 1 is not limited to sheets manufactured by this manufacturing method.

[0123] The present pressure-sensitive adhesive sheet 1 can be produced by preparing a pressure-sensitive adhesive composition containing an acrylic polymer (A), preferably a crosslinking agent (B), a photoinitiator (C), and other components as necessary, forming the pressure-sensitive adhesive composition into a sheet, curing it by crosslinking, i.e., polymerization, and then processing it appropriately as necessary.

[0124] The pressure-sensitive adhesive composition may be prepared by kneading the raw materials using a temperature-controllable kneader (for example, a single-screw extruder, a twin-screw extruder, a planetary mixer, a twin-screw mixer, a pressure kneader, etc.). When kneading the various raw materials, various additives such as a silane coupling agent and an antioxidant may be blended together with a resin in advance and then fed to the kneader, or all materials may be melt-mixed in advance and then fed, or a masterbatch in which only the additives are concentrated in a resin may be prepared in advance and then fed.

[0125] The pressure-sensitive adhesive composition can be formed into a sheet by any known method, such as wet lamination, dry lamination, extrusion casting using a T-die, extrusion lamination, calendaring, inflation, injection molding, and liquid injection curing. Among these, when producing a sheet, wet lamination, extrusion casting, and extrusion lamination are preferred.

[0126] The pressure-sensitive adhesive composition can be cured by irradiating it with active energy rays, and the pressure-sensitive adhesive sheet 1 can be produced by irradiating a molded product of the pressure-sensitive adhesive composition, for example, a sheet, with active energy rays. In addition to irradiating it with active energy rays, the composition can also be further cured by heating.

[0127] Furthermore, the irradiation energy, irradiation time, irradiation method, etc. of the active energy rays are not particularly limited as long as they can activate the photoinitiator (C) and polymerize photoreactive components such as (meth)acrylic acid ester compounds. When a hydrogen abstraction photoinitiator is used as the photoinitiator (C), a hydrogen abstraction reaction also occurs from the acrylic polymer (A), and the acrylic polymer (A) is incorporated into the crosslinked structure, forming a crosslinked structure with many crosslinking points. Therefore, it is preferable that the pressure-sensitive adhesive sheet 1 be cured using a hydrogen abstraction photoinitiator.

[0128] Examples of the active energy rays in the active energy ray irradiation include light rays such as far ultraviolet rays, ultraviolet rays, near ultraviolet rays, infrared rays, and visible light rays, as well as ionizing radiation such as X-rays, α-rays, β-rays, γ-rays, electron beams, proton beams, and neutron beams. Among these, ultraviolet rays are preferred from the viewpoints of suppressing damage to optical device components and controlling reactions. Furthermore, ultraviolet rays are preferred from the viewpoints of curing speed, ease of availability of an irradiation device, cost, and the like.

[0129] Examples of light sources for ultraviolet irradiation include high-pressure mercury lamps, ultra-high-pressure mercury lamps, low-pressure mercury lamps, carbon arc lamps, metal halide lamps, xenon lamps, chemical lamps, electrodeless discharge lamps, and LED lamps, all of which emit light in the wavelength range of 150 to 450 nm. Of these, it is preferable to use high-pressure mercury lamps, metal halide lamps, and LED lamps.

[0130] The amount of active energy ray irradiation (cumulative light amount) is 100 to 10,000 mJ / cm from the viewpoint of curing. 2 is preferred, and more preferably 200 to 8000 mJ / cm 2 , more preferably 200 to 6000 mJ / cm 2 This is carried out under the following conditions.

[0131] The present pressure-sensitive adhesive sheet 1 can also be provided as a pressure-sensitive adhesive sheet with a release film laminated on one or both sides thereof. In particular, from the viewpoint of preventing blocking and adhesion of foreign matter, it is preferable to coat both sides of the pressure-sensitive adhesive sheet 1 with a release film.

[0132] When release films are provided on both sides of the present pressure-sensitive adhesive sheet 1, a laminate configuration in which a light release film with a relatively low release strength and a heavy release film with a relatively high release strength are laminated is preferred. When using a pressure-sensitive adhesive sheet with release films provided on both sides, first, one release film (light release film) is peeled off to expose one side of the pressure-sensitive adhesive sheet, which is then bonded to a component of an image display device (referred to as a first component), and the other release film (heavy release film) is peeled off to expose the other side of the pressure-sensitive adhesive sheet, which is then bonded to a component of an image display device (referred to as a second component).

[0133] As such a release film, a known release film can be appropriately used. As the base material of the release film, for example, a film such as a polyester film, a polyolefin film, a polycarbonate film, a polystyrene film, an acrylic film, a triacetyl cellulose film, or a fluororesin film that has been subjected to a release treatment by coating with a release agent such as a silicone resin, or release paper, etc., can be appropriately selected and used. Among these, a polyester film is preferred, a polyethylene terephthalate (PET) film is more preferred, and a biaxially oriented PET film is particularly preferred because of its excellent transparency, mechanical strength, heat resistance, flexibility, etc. Furthermore, a release film can be used in which a release layer formed by curing a curable silicone-based release agent containing a silicone resin as a main component is provided on the base material.

[0134] The thickness of the release film is not particularly limited, but from the viewpoint of processability and handling, the thickness is preferably 10 to 250 μm, more preferably 25 to 200 μm, and even more preferably 35 to 190 μm.

[0135] In another embodiment of the method for producing the present pressure-sensitive adhesive sheet 1, the pressure-sensitive adhesive composition can be dissolved in an appropriate solvent and various coating methods can be used. When a coating method is used, the present pressure-sensitive adhesive sheet 1 can also be obtained by thermal curing in addition to the above-mentioned curing by irradiation with active energy rays. When a coating method is used, the thickness of the present pressure-sensitive adhesive sheet 1 can be adjusted by the coating thickness and the solids concentration of the coating liquid.

[0136] The coating method may be a conventional method such as roll coating, die coating, gravure coating, comma coating, screen printing, or bar coating.

[0137] To produce the present pressure-sensitive adhesive sheet 1 using the coating method, for example, the pressure-sensitive adhesive composition can be dissolved in a solvent, coated on the release film, dried, and cured by active energy ray irradiation to form the present pressure-sensitive adhesive sheet 1. Furthermore, a release film may be laminated on top as necessary. In this case, the pressure-sensitive adhesive composition may be coated on a release film, dried, cured by active energy ray irradiation, and then a release film may be laminated on top of that, or the pressure-sensitive adhesive sheet 1 may be formed by coating on a release film, drying, laminating a release film, and then curing by active energy ray irradiation.

[0138] The solvent is not particularly limited as long as it dissolves the pressure-sensitive adhesive composition, and examples thereof include ester solvents such as methyl acetate, ethyl acetate, butyl acetate, methyl acetoacetate, and ethyl acetoacetate; ketone solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; aromatic solvents such as toluene and xylene; and alcohol solvents such as methanol, ethanol, and propyl alcohol. These can be used alone or in combination of two or more. Among them, ethyl acetate, acetone, methyl ethyl ketone, and toluene are preferred in terms of solubility, drying properties, cost, and the like, and ethyl acetate is particularly preferred.

[0139] In view of drying properties, the content of the solvent is preferably 600 parts by mass or less, more preferably 500 parts by mass or less, even more preferably 400 parts by mass or less, and particularly preferably 300 parts by mass or less, relative to 100 parts by mass of the acrylic polymer (A), while being preferably 1 part by mass or more, more preferably 50 parts by mass or more, even more preferably 100 parts by mass or more, and particularly preferably 150 parts by mass or more.

[0140] The solvent content in the pressure-sensitive adhesive composition after drying is preferably 1% by mass or less, more preferably 0.5% by mass or less, particularly preferably 0.1% by mass or less, and most preferably 0% by mass.

[0141] The drying temperature is usually 40 to 150° C., more preferably 45 to 140° C., even more preferably 50 to 130° C., and particularly preferably 55 to 120° C. When the temperature is within this range, the solvent can be removed efficiently and relatively safely while suppressing thermal deformation of the release film.

[0142] The drying time is usually 1 to 30 minutes, more preferably 3 to 25 minutes, and even more preferably 5 to 20 minutes. When the drying time is within this range, the solvent can be removed efficiently and sufficiently.

[0143] Drying methods include, for example, drying with a dryer, drying with a heated roll, drying by blowing hot air onto the film, etc. Among these, using a dryer is preferred because it allows for uniform and easy drying. These methods can be used alone or in combination of two or more.

[0144] In yet another embodiment of the method for producing the present pressure-sensitive adhesive sheet 1, a pressure-sensitive adhesive composition may be prepared, coated onto a component of an image display device described below, and then cured to produce the present pressure-sensitive adhesive sheet 1. However, the method is not limited to this.

[0145] Furthermore, the present pressure-sensitive adhesive sheet 1 may be a single-layer pressure-sensitive adhesive sheet consisting of only an acrylic pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition, or may be a multi-layer pressure-sensitive adhesive sheet in which multiple other acrylic pressure-sensitive adhesive layers or other pressure-sensitive adhesive layers are laminated. Among these, the layer structure of the present pressure-sensitive adhesive sheet 1 is preferably a single layer from the viewpoints of ease of production and ease of reducing adhesive extrusion. On the other hand, from the viewpoint of tending to provide a pressure-sensitive adhesive sheet that is less likely to leave indentations or dents even when localized pressure is applied, it is preferably at least two layers, more preferably having at least three layers: an outermost layer, a backmost layer, and an intermediate layer, and particularly preferably having at least three layers in which the outermost layer and the backmost layer are acrylic pressure-sensitive adhesive layers.

[0146] When the pressure-sensitive adhesive sheet 1 has at least three layers, namely, a surface layer, a back layer, and an intermediate layer, the surface layer and the back layer (hereinafter also referred to as "surface and back layers") and the intermediate layer (the layer sandwiched between the surface layer and the back layer) are preferably formed from a pressure-sensitive adhesive composition containing acrylic polymers (A) of different compositions, particularly containing acrylic polymers (A) of different compositions as the main component. Such a layer configuration is advantageous in that contradictory physical properties such as stress relaxation and shape retention can be functionally separated for each layer. Furthermore, the surface layer and the back layer may be formed from a pressure-sensitive adhesive composition containing acrylic polymers (A) of different compositions, particularly containing acrylic polymers (A) of different compositions as the main component, but are preferably formed from a pressure-sensitive adhesive composition containing acrylic polymers (A) of the same composition.

[0147] When the pressure-sensitive adhesive sheet 1 has at least three layers (top layer / intermediate layer / rearmost layer) in which the top layer and the rearmost layer are acrylic pressure-sensitive adhesive layers, the top layer and the rearmost layer (surfaces to be attached to components of an image display device) are preferably high Tg layers. The intermediate layer sandwiched between the top layer and the rearmost layer is preferably a low Tg layer. Furthermore, the high Tg layers used in the top layer and the rearmost layer may have different glass transition temperatures (Tg), but the top layer and the rearmost layer preferably have the same glass transition temperature, and it is particularly preferred that the top layer and the rearmost layer be acrylic pressure-sensitive adhesive layers formed from the same pressure-sensitive adhesive composition.

[0148] The high Tg layer refers to a layer whose maximum value (glass transition temperature) of loss tangent (Tan δ) obtained by dynamic viscoelasticity measurement in the shear mode is usually −25° C. or higher, preferably −10° C. or higher, and particularly preferably 0° C. or higher. The upper limit of the glass transition temperature of the high Tg layer is usually 60° C. or lower, preferably 40° C. or lower, more preferably 20° C. or lower, and even more preferably 10° C. or lower. The low Tg layer refers to a layer whose maximum value (glass transition temperature) of loss tangent (Tan δ) obtained by dynamic viscoelasticity measurement in the shear mode is lower than the glass transition temperature of the high Tg layer, and whose glass transition temperature is usually 20° C. or lower, preferably 15° C. or lower, more preferably 10° C. or lower, even more preferably 8° C. or lower, particularly preferably 5° C. or lower, and most preferably 0° C. or lower. The lower limit of the glass transition temperature of the low Tg layer is usually −80° C., preferably −60° C. or higher, more preferably −50° C. or higher, and even more preferably −40° C. or higher.

[0149] Furthermore, when the pressure-sensitive adhesive sheet 1 has at least three layers, the outermost and innermost layers of which are acrylic pressure-sensitive adhesive layers, the ratio of the total thickness of the outermost and innermost layers to the total thickness is preferably 5 to 70%, more preferably 10 to 60%, and particularly preferably 20 to 45%. By setting the thicknesses of the outermost and innermost layers within the above ranges, a pressure-sensitive adhesive sheet can be obtained that is excellent in lamination suitability and durability, such as resistance to foaming at the peripheral edge, resistance to adhesive extrusion, and level difference absorbency.

[0150] The pressure-sensitive adhesive sheet 1 thus obtained is an optically transparent pressure-sensitive adhesive sheet. Here, "optically transparent" means that the total light transmittance is 80% or more, preferably 85% or more, and more preferably 90% or more. The haze value of the pressure-sensitive adhesive sheet is preferably 10% or less, more preferably 5% or less, and particularly preferably 3% or less.

[0151] The thickness of the present pressure-sensitive adhesive sheet is preferably 50 to 1000 μm, more preferably 60 to 500 μm, and particularly preferably 75 to 300 μm.

[0152] Furthermore, the pressure-sensitive adhesive sheet 1 may be embossed or processed to have various irregularities (such as conical, pyramidal, or hemispherical shapes) as needed. Furthermore, in order to improve adhesion to various members, the surface may be subjected to various surface treatments such as corona treatment, plasma treatment, and primer treatment.

[0153] <Present Pressure-Sensitive Adhesive Sheet 2> As described above, the present pressure-sensitive adhesive sheet 2 has an acrylic pressure-sensitive adhesive layer, which is a cured reaction product formed from a syrup composition containing an alkyl(meth)acrylate (a1) and a hydroxyl group-containing monomer (a2). Each component contained in the acrylic pressure-sensitive adhesive layer (syrup composition) will be described in detail below.

[0154] [Alkyl (meth)acrylate (a1)] Examples of the alkyl (meth)acrylate (a1) include the alkyl (meth)acrylate (a1) described in the present adhesive sheet 1, and the types of preferred monomers are also the same as those of the alkyl (meth)acrylate (a1) described in the present adhesive sheet 1.

[0155] The content of the structural units derived from the alkyl (meth)acrylate (a1) is preferably 5 to 95% by mass, more preferably 10 to 90% by mass, even more preferably 15 to 85% by mass, and particularly preferably 20 to 80% by mass, relative to the acrylic pressure-sensitive adhesive layer (syrup composition) in order to obtain flexibility. When the content of the structural units derived from the alkyl (meth)acrylate (a1) is equal to or greater than the lower limit, excellent resistance to foaming at the peripheral edge during lamination is obtained, and when the content is equal to or less than the upper limit, it is preferable in terms of achieving compatibility with other physical properties such as adhesiveness.

[0156] [Hydroxyl Group-Containing Monomer (a2)] Examples of the hydroxyl group-containing (meth)acrylate (a2) include the hydroxyl group-containing monomer (a2) described in the present adhesive sheet 1, and the types of preferred monomers are also the same as those of the hydroxyl group-containing (meth)acrylate (a2) described in the present adhesive sheet 1.

[0157] The content of the structural unit derived from the hydroxyl group-containing monomer (a2) is usually 3 to 30% by mass, preferably 5 to 25% by mass, and particularly preferably 7 to 20% by mass, relative to the acrylic pressure-sensitive adhesive layer (syrup composition). If the content is too low, the adhesive strength and moist heat resistance when used as a pressure-sensitive adhesive tend to decrease, while if the content is too high, the pressure-sensitive adhesive layer is more likely to undergo a self-crosslinking reaction, which tends to decrease heat resistance.

[0158] The syrup composition may also contain the copolymerizable monomers (a3) ​​to (a10) described above in connection with the present pressure-sensitive adhesive sheet 1. The types of these preferred monomers are the same as those described above in connection with the present pressure-sensitive adhesive sheet 1. The preferred content of the structural units derived from these copolymerizable monomers (a3) ​​to (a10), i.e., the mass ratio relative to the total mass of the acrylic pressure-sensitive adhesive layer (syrup composition), is the same as the mass ratio relative to all structural units of the acrylic polymer (A) described above in connection with the present pressure-sensitive adhesive sheet 1.

[0159] Furthermore, the acrylic adhesive layer preferably contains the crosslinking agent (B) and photoinitiator (C) described above in the present adhesive sheet 1, and may also contain other components such as a silane coupling agent, described above in the present adhesive sheet 1.

[0160] [Crosslinking Agent (B)] When the crosslinking agent (B) is used, the preferred compounds and physical properties are the same as those of the crosslinking agent (B) described above for the present pressure-sensitive adhesive sheet 1. The preferred content of the crosslinking agent (B) is usually 0.1 to 20 mass%, preferably 0.5 to 15 mass%, and particularly preferably 1 to 10 mass%, relative to the acrylic pressure-sensitive adhesive layer (syrup composition). When the content is equal to or greater than the lower limit, poor curing tends to be prevented, while when the content is equal to or less than the upper limit, the film tends to have appropriate flexibility and excellent stress relaxation properties.

[0161] [Photoinitiator (C)] The photoinitiator is not particularly limited as long as it is the photoinitiator described above in the present pressure-sensitive adhesive sheet 1, but from the viewpoint of efficiently progressing the polymerization reaction, it is preferable to include a cleavage-type photoinitiator, and among the above-mentioned cleavage-type photoinitiators, 2,2-dimethoxy-1,2-diphenylethan-1-one, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and (2,4,6-trimethylbenzoyl)ethoxyphenylphosphine oxide are particularly preferred. Furthermore, from the viewpoint of efficiently forming a crosslinked structure, it is preferable to include a hydrogen abstraction-type photoinitiator, and benzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, 4-phenylbenzophenone, 3,3'-dimethyl-4-methoxybenzophenone, and 4-(meth)acryloyloxybenzophenone are particularly preferred. The photoinitiator (C) may include one or more selected from the group consisting of cleavage-type photoinitiators and / or hydrogen abstraction-type photoinitiators.

[0162] When the photoinitiator (C) is used, its content is usually 0.1 to 10% by mass, preferably 0.5 to 6% by mass, and more preferably 1 to 4% by mass, relative to the acrylic pressure-sensitive adhesive layer (syrup composition). When the content is equal to or greater than the lower limit, poor curing tends to be prevented, while when the content is equal to or less than the upper limit, deterioration in stability such as precipitation from the pressure-sensitive adhesive sheet tends to be suppressed, and problems such as embrittlement and coloration tend to be suppressed.

[0163] [Monofunctional (meth)acrylate] When a monofunctional (meth)acrylate is used, the preferred compounds and physical properties are the same as those explained for the present pressure-sensitive adhesive sheet 1 above.

[0164] [Other Components] The other components may be the same as those described above for the present pressure-sensitive adhesive sheet 1. In particular, when a silane coupling agent is used, its content is usually 0.005 to 5 mass %, preferably 0.01 to 3 mass %, and more preferably 0.05 to 1 mass %, relative to the acrylic pressure-sensitive adhesive layer (syrup composition). When the content is within the above range, adhesive strength and durability tend to be improved.

[0165] The syrup component constituting the syrup composition in the present pressure-sensitive adhesive sheet 2 may be composed of an acrylic polymer (A) and a monomer component. In one example, such a syrup component may be formed by partial polymerization of the so-called monomer component, or may be prepared by adding the monomer component to a polymer in which the monomer components constituting the acrylic polymer (A) are completely or partially polymerized. That is, when a predetermined copolymerization component is partially polymerized, some of the monomers polymerize to form oligomers or polymers, while some of the monomers remain, thereby forming a syrup component. In another example, a syrup-like state can be obtained by adding the monomer component to a partially or completely polymerized polymer. Therefore, the term "monomer unit constituting the acrylic pressure-sensitive adhesive layer" as used herein may refer to a monomer present in the acrylic polymer component in the form of an oligomer or polymer, or a monomer contained in the syrup component before polymerization.

[0166] <Method for manufacturing the present pressure-sensitive adhesive sheet 2> Next, a description will be given of a method for manufacturing the present pressure-sensitive adhesive sheet 2. However, the following description is an example of a method for manufacturing the present pressure-sensitive adhesive sheet 2, and the present pressure-sensitive adhesive sheet 2 is not limited to sheets manufactured by this manufacturing method.

[0167] In producing the present pressure-sensitive adhesive sheet 2, a syrup composition is typically prepared by mixing an alkyl (meth)acrylate (a1) having an alkyl group containing 3 to 30 carbon atoms, a hydroxyl group-containing monomer (a2), and optionally copolymerizable monomers (a3) ​​to (a10), a photoinitiator (C), and the like. This syrup composition is then irradiated with active energy rays to allow prepolymerization. The syrup composition, to which additional photoinitiator (C), crosslinker (B), and other components are added as needed, is then coated onto a release film or the like using various coating methods, and the resulting composition is then cured by irradiation with active energy rays or heating to obtain the present pressure-sensitive adhesive sheet 2. The crosslinker and other components may be added to the syrup composition from the beginning, or may be added to the syrup composition after prepolymerization has been completed. Furthermore, prepolymerization and curing may be performed in a single step.

[0168] In another embodiment of the method for manufacturing the present adhesive sheet 2, the syrup composition is dissolved in a solvent, then coated on a release film and dried, and then prepolymerized and cured by irradiation with active energy rays, thereby forming the present adhesive sheet 2.

[0169] In the manufacturing method of the present pressure-sensitive adhesive sheet 2, the release film, active energy rays, solvent, etc., mixing method, coating method, drying conditions, etc. may be the same as those described in the manufacturing method of the present pressure-sensitive adhesive sheet 1 above.

[0170] The present pressure-sensitive adhesive sheet 2 obtained in this manner may be a single-layer sheet having only an acrylic pressure-sensitive adhesive layer, or a multi-layer sheet having multiple acrylic pressure-sensitive adhesive layers and other pressure-sensitive adhesive layers laminated thereon. The preferred layer configuration and thickness are the same as those of the present pressure-sensitive adhesive sheet 1. The present pressure-sensitive adhesive sheet 2 can also be provided as a pressure-sensitive adhesive sheet with a release film, which has a configuration in which a release film is laminated on one or both sides of an adhesive layer (the present pressure-sensitive adhesive sheet) made of a pressure-sensitive adhesive composition.

[0171] <Preferred uses of the present pressure-sensitive adhesive sheet> The present pressure-sensitive adhesive sheets 1 and 2 are preferably used for bonding optical components. Specifically, they are preferably used for bonding components constituting a display, particularly components used to manufacture a display, and are preferably used as pressure-sensitive adhesive sheets for bonding image display device components such as an image display panel and a protective panel or touch panel arranged on the front side (viewing side) of the image display device, or components constituting the image display device components. Note that the same image display device components as those described below can be used.

[0172] <<Laminate for Image Display Device>> A laminate for an image display device according to one example of the embodiment of the present invention (hereinafter, may be referred to as "the present laminate for an image display device") is a laminate for an image display device having a configuration in which two components of the image display device are laminated with the present pressure-sensitive adhesive sheet interposed therebetween. The present laminate for an image display device is preferably a laminate for an image display device having a configuration in which two components of the image display device are laminated with the present pressure-sensitive adhesive sheet interposed therebetween.

[0173] Of the components of the present laminate for an image display device, the present pressure-sensitive adhesive sheet has been described above, and the components other than the pressure-sensitive adhesive sheet will be described below.

[0174] <Image Display Device Components> Examples of image display device components constituting the present laminate for an image display device include flat panel image display device components, curved image display device components, and flexible image display device components. Examples of such image display device components include image display panels such as liquid crystal displays and organic electroluminescence (EL) displays, surface protection panels (surface protection films), polarizing plates, polarizing elements, retardation films, color filters, barrier films, viewing angle compensation films, brightness enhancement films, contrast enhancement films, diffusion films, semi-transmitting reflective films, electrode films, transparent conductive films, metal mesh films, and touch sensor films. Any one of these may be used alone or in combination. Examples include a combination of a surface protection panel with another image display device component, or a combination with another image display device component.

[0175] Preferably, one of the two image display device components is a surface protection panel, and the other is a component consisting of one or a combination of two or more of the following: a touch sensor film, an image display panel, a color filter, a polarizing element, and a retardation film. It is more preferable that the surface protection panel has a frame-shaped concealing portion on its periphery, with the frame having a portion with a width of 3 mm or less. With this configuration, the effects of the present invention can be particularly achieved. From this perspective, a panel having a portion with a frame width of 2 mm or less is particularly preferable, and a panel having a portion with a width of 1.5 mm or less is particularly preferable.

[0176] The present laminate for an image display device is preferably fixed in a curved shape. Since the present pressure-sensitive adhesive sheet also has excellent reliability in laminating to curved parts, the above-mentioned configuration allows the effects of the present invention to be particularly enjoyed.

[0177] <Method for manufacturing the present laminate for an image display device> The method for manufacturing the present laminate for an image display device is not particularly limited, and as described above, for example, the pressure-sensitive adhesive composition may be applied to a component of an image display device to form a pressure-sensitive adhesive sheet, or a pressure-sensitive adhesive sheet with a release film may be formed in advance and then laminated to a component of an image display device.

[0178] <<Image Display Device>> An image display device according to an embodiment of the present invention (hereinafter, sometimes referred to as the "image display device") incorporates a laminate for an image display device, which has a configuration in which two image display device components are bonded together via the present pressure-sensitive adhesive sheet. For example, an image display device may have a structure in which a laminate for an image display device, which has a configuration in which two image display device components are bonded together via the present pressure-sensitive adhesive sheet, is combined with other image display device components. In this case, "other image display device components" may include, for example, FPC cables, reflective sheets, light guide plates and light sources, diffusion films, prism sheets, liquid crystal panels, organic EL panels, anti-reflection films, color filters, polarizing plates, retardation plates, glass substrates, surface protection films, and integrated composites of these components. Specific examples of the image display device include liquid crystal displays, organic EL displays, inorganic EL displays, electronic paper, plasma displays, and microelectromechanical system (MEMS) displays used in personal computers, mobile devices, game consoles, televisions (TVs), car navigation systems, touch panels, pen tablets, etc.

[0179] The present invention will be explained in more detail below by way of examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the invention.

[0180] Prior to the examples, the following raw materials were prepared.

[0181] [Acrylic Polymer (A)] Acrylic polymers (A-1) to (A-3) having copolymer component compositions and weight average molecular weights (Mw) as shown in Table 1 below were prepared.

[0182]

[0183] <Crosslinking Agent (B)> (B-1): Polypropylene glycol #400 diacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd., "NK Ester APG-400") (B-2): Hexanediol diacrylate (B-3): Propoxylated pentaerythritol tri- and tetraacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd., "NK Ester ATM-4PL")

[0184] <Photoinitiator (C)> (C-1): Methylbenzoyl formate ("Omnirad MBF" manufactured by IGM) (C-2): 4-methallyloyloxybenzophenone ("MBP" manufactured by Shinryo Corporation) (C-3): 4-acryloyloxybenzophenone (manufactured by Shanghai Shaoyi Biotechnology Co., Ltd.) (C-4): Benzyl dimethyl ketal ("Omnirad 651" manufactured by IGM) (C-5): Mixture of 2,4,6-trimethylbenzophenone and 4-methylbenzophenone ("Esacure TZT" manufactured by IGM)

[0185] <Others> Silane coupling agent: 3-glycidyloxypropyltrimethoxysilane ("KBM403" manufactured by Shin-Etsu Chemical Co., Ltd.)

[0186] Example 1 A pressure-sensitive adhesive composition was prepared by uniformly mixing 100 parts by mass of a (meth)acrylic polymer (A-1), 1.5 parts by mass of a crosslinking agent (B-1), 2.45 parts by mass of a photoinitiator (C-1), 1.05 parts by mass of a photoinitiator (C-2), and 0.2 parts by mass of a silane coupling agent.

[0187] Next, the pressure-sensitive adhesive composition was spread in a sheet form on a 100 μm-thick release film (PET film manufactured by Mitsubishi Chemical Corporation) that had been subjected to a silicone release treatment so that the thickness of the pressure-sensitive adhesive composition was 150 μm. In addition, a 75 μm-thick release film (PET film manufactured by Mitsubishi Chemical Corporation) that had been subjected to a silicone release treatment was laminated on the sheet-like pressure-sensitive adhesive composition. Thereafter, a high-pressure mercury lamp was used to irradiate the pressure-sensitive adhesive composition with an integrated light intensity of 2250 mJ / cm at a wavelength of 365 nm. 2 Both surfaces of the sheet-shaped pressure-sensitive adhesive composition were irradiated with active energy rays through the release film to obtain a pressure-sensitive adhesive sheet with a release film consisting of release film / pressure-sensitive adhesive sheet / release film.

[0188] Examples 2 to 4 PSA sheets with release films were prepared in the same manner as in Example 1, except that the formulation, thickness and integrated light amount were changed as shown in Table 2 below.

[0189] Example 5 100 parts by mass of an acrylic polymer (A-1), 1.5 parts by mass of a crosslinker (B-1), 2.45 parts by mass of a photoinitiator (C-1), 1.05 parts by mass of a photoinitiator (C-2), and 0.2 parts by mass of a silane coupling agent were prepared and uniformly mixed to form a pressure-sensitive adhesive composition for the front and back layers. On the other hand, 100 parts by mass of an acrylic polymer (A-3), 1.5 parts by mass of a crosslinker (B-1), 1.75 parts by mass of a photoinitiator (C-1), and 0.75 parts by mass of a photoinitiator (C-2) were prepared and uniformly mixed to form a pressure-sensitive adhesive composition for the intermediate layer. The pressure-sensitive adhesive composition for the front and back layers and the pressure-sensitive adhesive composition for the intermediate layer were each fed into two extruders and co-extruded in a two-kind, three-layer structure (outermost layer / intermediate layer / outermost layer, thickness ratio 1:2:1), followed by hot-melt molding into a 150 μm-thick sheet.

[0190] Next, the sheet-like pressure-sensitive adhesive composition was sandwiched between two polyethylene terephthalate films (a PET film manufactured by Mitsubishi Chemical Corporation, thickness 100 μm, and a PET film manufactured by Mitsubishi Chemical Corporation, thickness 75 μm) whose surfaces had been treated with silicone release agent, i.e., two release films, to obtain a laminate consisting of a release film / pressure-sensitive adhesive composition / release film. Thereafter, a high-pressure mercury lamp was used to irradiate the laminate with an integrated light intensity of 2250 mJ / cm at a wavelength of 365 nm. 2 Both surfaces of the sheet-shaped pressure-sensitive adhesive composition were irradiated with active energy rays through the release film to obtain a pressure-sensitive adhesive sheet with a release film consisting of release film / pressure-sensitive adhesive sheet / release film.

[0191] Comparative Example 1 A pressure-sensitive adhesive sheet with a release film was produced in the same manner as in Example 1, except that the formulation, thickness and integrated light amount were changed to those shown in Table 2 below.

[0192]

[0193] [Measurement and Evaluation of Physical Properties] The pressure-sensitive adhesive sheets prepared in the above Examples and Comparative Examples were subjected to the following various measurements and evaluations. The evaluation results are summarized in Table 3 below.

[0194] [25°C Shear Storage Modulus (G')] The release film on one side was removed from the pressure-sensitive adhesive sheets with release films prepared in the Examples and Comparative Examples, and the sheets were repeatedly laminated with a hand roller to a thickness of approximately 0.8 mm, and then punched out into circles with a diameter of 8 mm to prepare samples. The obtained samples were placed in a rheometer (T.A. Instruments' "DHR-2"), and dynamic viscoelasticity measurements were performed under the conditions of a measuring jig: 8 mm diameter parallel plates, a frequency of 1 Hz, a measuring temperature of -50 to 150°C, and a heating rate of 5°C / min, and the shear storage modulus (G') at 25°C was read.

[0195] [Glass transition temperature] The release film on one side of the pressure-sensitive adhesive sheet with release film prepared in the Examples and Comparative Examples was removed, and the sheet was repeatedly laminated with a hand roller to a thickness of approximately 0.8 mm. A circle with a diameter of 8 mm was punched out to prepare a sample. The obtained sample was placed in a rheometer ("DHR-2" manufactured by T.A. Instruments) and subjected to dynamic viscoelasticity measurement under the following conditions: measurement jig: 8 mm diameter parallel plate; frequency: 1 Hz; measurement temperature: -50 to 150 ° C; heating rate: 5 ° C / min. The glass transition temperature (Tg), defined as the maximum value of Tan δ obtained by dynamic viscoelasticity measurement in shear mode at a frequency of 1 Hz, was determined.

[0196] [Stress Relaxation Rate] The release film on one side was removed from the pressure-sensitive adhesive sheets with release film prepared in the Examples and Comparative Examples, and the sheets were repeatedly laminated with a hand roller to a thickness of approximately 0.8 mm. A circle with a diameter of 8 mm was punched out to prepare a sample. A viscoelasticity measuring device ("DHR2" manufactured by T.A. Instruments) was used to apply a 25% strain to the obtained sample at 70°C, and the storage modulus after 0.1 seconds was read as the initial modulus (G'(0)). A 25% strain was also applied at 70°C, and the storage modulus after 300 seconds was read as the relaxation modulus (G'(300)). The values ​​of the initial modulus (G'(0)) and the relaxation modulus (G'(300)) were substituted into the following formula (I) to determine the stress relaxation rate. Stress relaxation rate = (G'(300) / G'(0)) (I)

[0197] [Gel Fraction] For the pressure-sensitive adhesive sheets with release films prepared in the Examples and Comparative Examples, approximately 0.1 g of pressure-sensitive adhesive sheet pieces were collected from the pressure-sensitive adhesive sheets after peeling off the release films. The collected pressure-sensitive adhesive sheet pieces were wrapped in a pre-formed bag of SUS mesh (#150) with a mass (X), and the bag was closed to prepare a sample, and the mass (Y) of the sample was measured. The sample was immersed in ethyl acetate and stored in a dark place at 23°C for 24 hours, and then removed and heated at 70°C for 4.5 hours to evaporate the ethyl acetate, and the mass (Z) of the dried sample was measured. The measured masses were substituted into the following formula (2) to calculate the gel fraction before irradiation with active energy rays. Gel fraction (%) = [(Z-X) / (Y-X)] x 100

[0198] [Adhesive Strength] The release film on one side of the adhesive sheet with release film prepared in the Examples and Comparative Examples was removed, and a PET film (Cosmoshine A4300, manufactured by Toyobo Co., Ltd., thickness 100 μm) was attached as a backing film using a hand roller. This was cut into strips 10 mm wide x 150 mm long, and the remaining release film was peeled off, and the exposed adhesive sheet surface was attached to the surface of soda lime glass using a hand roller. The resulting laminate was autoclaved (60 ° C, gauge pressure 0.2 MPa, 20 minutes) for finish attachment to prepare an adhesive strength measurement sample. The obtained adhesive strength measurement sample was peeled from the soda lime glass together with the backing film while being pulled at an angle of 180 ° at a peeling rate of 60 mm / min under conditions of 23 ° C, 50% RH, and the adhesive sheet was peeled off from the soda lime glass at an angle of 180 ° C, and the tensile strength (N / cm) was measured using a load cell to determine the adhesive strength.

[0199] [Adhesive overflow distance] The release film on one side of the adhesive sheets with release film produced in the Examples and Comparative Examples was peeled off and the sheets were half-cut to 10 mm x 10 mm. The exposed adhesive surface was placed opposite a 0.6 mm thick soda lime glass, and the adhesive sheet and glass were pressure-bonded using a vacuum laminator at a temperature of 23°C, a gauge pressure of 0.4 MPa, and a pressure-bonding time of 60 seconds. The distance that the adhesive overflowed from the half-cut marking line at the center of each side of the adhesive sheet was measured, and the average value of the four sides was taken as the adhesive overflow distance (μm).

[0200] [Bubble Resistance (Edge Bubble)] The pressure-sensitive adhesive sheets with release film prepared in the Examples and Comparative Examples were cut to 45 mm x 45 mm. The release film on one side of the cut pressure-sensitive adhesive sheet was removed, and the exposed adhesive surface was roll-pressed onto a soda-lime glass (54 mm x 82 mm x 0.6 mm thick). The remaining release film was then peeled off, and a polarizing plate (54 mm x 82 mm x 0.1 mm thick) was roll-laminated. The plate was then autoclaved (temperature 60°C, gauge pressure 0.2 MPa, 8 minutes) for finish lamination to prepare a sample for evaluating bubble resistance (edge ​​bubble). Eight evaluation samples were prepared for each example. The prepared samples were left to stand for 24 hours in an environment of 23°C and 50% RH, and then visually observed to determine the number of bubbles that had occurred within 1 mm of the edge of the pressure-sensitive adhesive sheet. The average number of edge bubbles per sample was calculated. Those in which no bubbles were found were rated as "◎ (very good)", those in which the average number of bubbles was 10 or less were rated as "◯ (good)", and those in which the average number of bubbles was more than 10 were rated as "× (poor)".

[0201]

[0202] The pressure-sensitive adhesive sheets of the Examples had a stress relaxation rate of 0.25 or more and were excellent in end surface foaming resistance. Among them, Examples 1, 2, and 5, which had a stress relaxation rate of more than 0.45, were particularly excellent in foaming resistance. On the other hand, the pressure-sensitive adhesive sheet of Comparative Example 1 had a low stress relaxation rate and was poor in end surface foaming resistance.

[0203] Although the above examples show specific embodiments of the present invention, the examples are merely illustrative and should not be construed as limiting. Various modifications that are obvious to those skilled in the art are intended to fall within the scope of the present invention.

[0204] The pressure-sensitive adhesive sheet of the present invention has excellent lamination properties and can be laminated without air bubbles up to the peripheral edge near the edge of the pressure-sensitive adhesive sheet, and therefore can be suitably used as a pressure-sensitive adhesive sheet for image display devices, particularly image display devices with narrow frame designs or frameless designs.

Claims

1. A pressure-sensitive adhesive sheet having an acrylic pressure-sensitive adhesive layer formed from a pressure-sensitive adhesive composition containing an acrylic copolymer (A), wherein the stress relaxation rate calculated from the initial elastic modulus (G'(0)) 0.1 seconds after application of a 25% strain at 70°C to the acrylic pressure-sensitive adhesive layer and the relaxed elastic modulus (G'(300)) 300 seconds after application of a 25% strain at 70°C using the following formula (I) is 0.25 or more. Stress relaxation rate = (G'(300) / G'(0)) ... (I) 2. An adhesive sheet having an acrylic adhesive layer, the acrylic adhesive layer being a cured reaction product formed from a syrup composition containing an alkyl (meth)acrylate (a1) having an alkyl group with 3 to 30 carbon atoms and a hydroxyl group-containing (meth)monomer (a2), the stress relaxation rate of the acrylic adhesive layer being 0.25 or more, calculated from the initial elastic modulus (G'(0)) 0.1 seconds after applying a 25% strain at 70°C and the relaxed elastic modulus (G'(300)) 300 seconds after applying a 25% strain at 70°C by the following formula (I): Stress relaxation rate = (G'(300) / G'(0)) ... (I) 3. The pressure-sensitive adhesive sheet according to claim 1 or 2, wherein the initial elastic modulus (G'(0)) is 5 to 100 kPa.

4. The pressure-sensitive adhesive sheet according to claim 1 or 2, wherein the relaxation elastic modulus (G'(300)) is 1.3 to 100 kPa.

5. The pressure-sensitive adhesive sheet according to claim 1 or 2, wherein the gel fraction of said pressure-sensitive adhesive sheet is 30 to 95%.

6. The pressure-sensitive adhesive sheet according to claim 1 or 2, which has a storage modulus (G'(25°C)) at a temperature of 25°C, as determined by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz, of 80 kPa or more.

7. The pressure-sensitive adhesive sheet according to claim 1 or 2, which has a glass transition temperature (Tg) defined as the maximum value of Tan δ obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz, of -20°C or higher.

8. The pressure-sensitive adhesive sheet according to claim 1 or 2, which is a single layer.

9. The pressure-sensitive adhesive sheet according to claim 1, wherein the pressure-sensitive adhesive composition contains a crosslinking agent (B) and a photoinitiator (C).

10. The adhesive sheet described in claim 9, wherein the photoinitiator (C) comprises a photoinitiator (c1) having within its molecule a radically polymerizable functional group having a carbon-carbon double bond and a structure that generates radicals, and a hydrogen abstraction type photoinitiator (c2) other than the photoinitiator (c1).

11. An adhesive sheet with a release film, comprising the adhesive sheet according to claim 1 or 2 and a release film laminated on the adhesive sheet.

12. A laminate for an image display device comprising two image display device components and an adhesive sheet according to claim 1 or 2 interposed between the two image display device components, one of the two image display device components being a surface protection panel and the other being a member consisting of any one or a combination of two or more of the group consisting of a touch sensor film, an image display panel, a color filter, a polarizing element, and a retardation film.

13. The laminate for an image display device according to claim 12, wherein the surface protection panel has a frame-shaped concealing portion on its periphery, the frame width of the concealing portion being 3 mm or less in some portions.

14. The laminate for an image display device according to claim 12, which is fixed in a curved shape.

15. An image display device comprising the laminate for an image display device according to claim 12.

16. An adhesive sheet for use as a component of an image display device, comprising the adhesive sheet according to claim 1 or 2.

Citation Information

Patent Citations

  • Pressure-sensitive adhesive sheet, method of manufacturing laminate and laminate

    JP2019077747A

  • Adhesive sheet and production method of the same, and method for manufacturing image display device

    JP2019131679A

  • Photocurable pressure-sensitive adhesive sheet laminate, method for manufacturing photocurable pressure-sensitive adhesive sheet laminate, and method for manufacturing image display panel laminate

    JP2019210446A

  • Adhesive sheet, laminated sheet and flexible image display device

    JP2023038851A

  • Adhesive Composition and Adhesive Sheet Using the Same

    KR102229885B1

Cited By

  • Laminate for constituting image display device, method for manufacturing same, and image display device constituent member with release film

    WO2026204932A1