Adhesive sheet, adhesive sheet with release film, laminated body for image display device, image display device, and adhesive sheet for component for image display device

The adhesive sheet addresses bonding reliability and air bubble issues in image display devices by using an acrylic adhesive with tailored properties, ensuring effective bonding in narrow frame and curved designs.

WO2024203790A1PCT designated stage expired Publication Date: 2024-10-03MITSUBISHI CHEM CORP

Patent Information

Application Number
PCT/JP2024/011179
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional adhesive sheets for image display devices face challenges in achieving high bonding reliability at the peripheral edges, particularly in narrow frame designs, where air bubbles and glue oozing are common issues due to the balance between flexibility and hardness, leading to reduced visibility and increased complexity in design.

Method used

A pressure-sensitive adhesive sheet with an acrylic adhesive layer, formulated to have specific elastic moduli, stress relaxation rates, and glass transition temperatures, combined with active energy ray curability, to ensure reliable bonding and prevent air bubbles and glue extrusion, suitable for curved and flat surfaces.

Benefits of technology

The adhesive sheet provides improved bonding reliability and resistance to air bubbles and glue oozing, enabling wider application in narrow frame designs and curved surfaces while maintaining flexibility and cohesive strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

The following is provided as an adhesive sheet that has a higher level of lamination reliability than the prior art. An adhesive sheet that has an acrylic adhesive layer formed from an adhesive composition containing an acrylic polymer (A), wherein the acrylic adhesive layer has a stress-relaxation rate (X0) of at most 0.20, which is calculated according to equation (I), in which (G0'(0)) is an initial elastic modulus that is observed after 0.1 seconds elapse after the application of a distortion of 25% to the acrylic adhesive layer at a temperature of 70°C, and (G0'(300)) is a relaxation elastic modulus that is observed after 300 seconds elapse after the application of a distortion of 25% to the acrylic adhesive layer at a temperature of 70°C. (I): Stress-relaxation rate (X0) = (G0'(300) / G0'(0))
Need to check novelty before this filing date? Find Prior Art

Description

Adhesive sheet, adhesive sheet with release film, laminate for image display device, image display device, and adhesive sheet for image display device constituent member

[0001] The present invention relates to a pressure-sensitive adhesive sheet, a pressure-sensitive adhesive sheet with a release film, a laminate for an image display device, an image display device, and a pressure-sensitive adhesive sheet for a component of an image display device.

[0002] In order to improve the visibility of image display devices, the gap between an image display panel such as a liquid crystal display (LCD), a plasma display (PDP), or an electroluminescence display (ELD) and a protective panel or touch panel member placed on the front side (viewing side) of the image display panel is filled with a resin such as an adhesive or glue, thereby suppressing reflection of incident light and outgoing light from the displayed image at the air layer interface.

[0003] For example, Patent Document 1 discloses a method for manufacturing a component laminate for an image display device, which has a configuration in which an image display device component is laminated on at least one side of a transparent double-sided adhesive sheet, in which an adhesive sheet that has been primarily crosslinked by ultraviolet light is attached to the image display device component, and then the adhesive sheet is irradiated with ultraviolet light through the image display device component to cause secondary curing.

[0004] Furthermore, Patent Document 2 discloses a pressure-sensitive adhesive sheet containing a (meth)acrylic copolymer having an ultraviolet-crosslinkable site, as a pressure-sensitive adhesive sheet useful for displays and touch panels.

[0005] Patent No. 4971529 Patent No. 6062740

[0006] There is a strong demand for image display devices to have as large an effective display area as possible without changing the external dimensions, i.e., to have a narrower frame. For this reason, there is also a demand for adhesive sheets for bonding image display components that can bond without air bubbles, even to the peripheral edge near the edge of the adhesive sheet, which in the past was located directly below the concealing part and was therefore not visible.

[0007] Furthermore, in recent years, there has been a demand for high design quality in image display devices, and the shape of the front surface protection panel is changing from flat to those with curved edges or corners, or to designs in which the entire display unit is curved, etc. In the case of curved members or members with curved edges or corners, air bubbles are more likely to occur around the periphery than in flat members.

[0008] The pressure-sensitive adhesive sheets in Patent Documents 1 and 2 were developed for laminated structures using conventional image display device components, and did not take into consideration the lamination reliability near the peripheral edge of the pressure-sensitive adhesive sheet, which would have been located directly below the concealed portion and therefore not visible in conventional cases. Furthermore, conventional flexible pressure-sensitive adhesive sheets tend to have crushed edges and the glue (adhesive layer) easily overflows. To address this issue, a certain degree of hardness is desirable, but excessive hardness can lead to the problem of air bubbles forming around the edges. Therefore, for image display devices with increasingly narrower picture frames, pressure-sensitive adhesive sheets that have an appropriate hardness yet offer better lamination reliability at the peripheral edge, which is a trade-off.

[0009] Therefore, in this context, the present invention provides an adhesive sheet, an adhesive sheet with a release film, a laminate for an image display device, an image display device, and an adhesive sheet for a component of an image display device, which have a higher level of bonding reliability than conventional ones.

[0010] That is, the present invention has the following aspects: [1] A pressure-sensitive adhesive sheet having an acrylic pressure-sensitive adhesive layer formed from a pressure-sensitive adhesive composition containing an acrylic polymer (A), wherein the acrylic pressure-sensitive adhesive layer has a stress relaxation modulus (X0) of 0.20 or less, calculated by the following formula (I) from the initial elastic modulus (G0'(0)) 0.1 second after applying a 25% strain at a temperature of 70°C to the acrylic pressure-sensitive adhesive layer and the relaxation modulus (G0'(300)) 300 seconds after applying a 25% strain at a temperature of 70°C to the acrylic pressure-sensitive adhesive layer: Stress relaxation rate (X0)=(G0'(300) / G0'(0)) (I) [2] A pressure-sensitive adhesive sheet having an acrylic pressure-sensitive adhesive layer, wherein the acrylic pressure-sensitive adhesive layer is a cured reaction product formed from a syrup composition containing an alkyl(meth)acrylate (a1) having an alkyl group with 3 to 30 carbon atoms, and a hydroxyl group-containing monomer (a2) and / or a nitrogen-containing monomer (a3), wherein the stress relaxation rate (X0) calculated by the following formula (I) from the initial elastic modulus (G0'(0)) 0.1 second after applying a 25% strain at a temperature of 70°C to the acrylic pressure-sensitive adhesive layer and the relaxed elastic modulus (G0'(300)) 300 seconds after applying a 25% strain at a temperature of 70°C to the acrylic pressure-sensitive adhesive layer is 0.20 or less. Stress relaxation modulus (X0) = (G0'(300) / G0'(0)) (I) [3] The pressure-sensitive adhesive sheet according to [1] or [2], wherein the relaxation modulus (G0'(0)) is 5 to 100 kPa. [4] The pressure-sensitive adhesive sheet according to any one of [1] to [3], wherein the relaxation modulus (G0'(300)) is 0.1 to 20 kPa. [5] The pressure-sensitive adhesive sheet according to any one of [1] to [4], wherein the shear storage modulus (G0'(25°C)) at a temperature of 25°C, obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz, is 100 kPa or more. [6] The pressure-sensitive adhesive sheet according to any one of [1] to [5], wherein the glass transition temperature (Tg0), defined as the maximum value of Tan δ, obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz, is -25°C or more. [7] The pressure-sensitive adhesive sheet according to any one of [1] to [6], wherein the pressure-sensitive adhesive sheet is active energy ray-curable. [8] The pressure-sensitive adhesive sheet is exposed to an active energy ray having a wavelength of 365 nm in an integrated light amount of 2000 to 4000 mJ / cm 2[7] The pressure-sensitive adhesive sheet according to [7], wherein the post-cure stress relaxation rate (X1) calculated by the following formula (II) from the post-cure initial elastic modulus (G1'(0)) 0.1 seconds after applying a 25% strain to the acrylic pressure-sensitive adhesive layer at a temperature of 70°C and the post-cure relaxation elastic modulus (G1'(300)) 300 seconds after applying a 25% strain to the acrylic pressure-sensitive adhesive layer at a temperature of 70°C is 0.22 or more. Post-cure stress relaxation rate (X1) = (G1'(300) / G1'(0)) (II) [9] The pressure-sensitive adhesive sheet according to [8], wherein the difference (X1 - X0) between the post-cure stress relaxation rate (X1) and the stress relaxation rate (X0) is 0.01 or more.

[10] The pressure-sensitive adhesive sheet according to [8], wherein the pressure-sensitive adhesive sheet is irradiated with active energy rays having a wavelength of 365 nm at an integrated light dose of 2000 to 4000 mJ / cm 2

[11] The pressure-sensitive adhesive sheet according to any one of [7] to [9], wherein the acrylic pressure-sensitive adhesive layer has an initial post-curing elastic modulus (G1'(0)) of 1 kPa or more and 100 kPa or less 0.1 seconds after applying a 25% strain at a temperature of 70°C when irradiated so as to satisfy the above condition. 2The pressure-sensitive adhesive sheet according to any one of [7] to

[10] , wherein the acrylic pressure-sensitive adhesive layer has a post-cure relaxation modulus (G1'(300)) of 0.1 kPa or more and 50 kPa or less 300 seconds after applying a 25% strain at a temperature of 70°C when irradiated so as to satisfy the condition.

[12] A pressure-sensitive adhesive sheet formed from a pressure-sensitive adhesive composition containing an acrylic polymer (A), wherein the pressure-sensitive adhesive sheet has a glass transition temperature (Tg0) defined by the maximum value of Tan δ obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz, of -40 to 20°C, and wherein the difference (ΔT) between the temperature (T1) at or below the glass transition temperature (Tg0) at which the shear storage modulus (G') and the loss modulus (G") become equal, and the temperature (T2) at or above the glass transition temperature (Tg0) at which the shear storage modulus (G') and the loss modulus (G") become equal, is 20°C or more.

[13] The pressure-sensitive adhesive sheet according to

[12] , wherein the maximum value of Tanδ is 1.2 or more.

[14] The pressure-sensitive adhesive sheet according to

[12] or

[13] , wherein the shear storage modulus (G0'(25°C)) at a temperature of 25°C, obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz, is 50 kPa or more.

[15] The pressure-sensitive adhesive sheet according to any one of

[12] to

[14] , which is active energy ray-curable.

[16] The pressure-sensitive adhesive sheet according to

[12] to

[14] , wherein the pressure-sensitive adhesive sheet is irradiated with active energy rays having a wavelength of 365 nm at an integrated light dose of 2000 to 4000 mJ / cm. 2

[17] The pressure-sensitive adhesive sheet according to

[15] , wherein the pressure-sensitive adhesive sheet has a shear storage modulus (G1'(25°C)) of 60 kPa or more at a temperature of 25°C, as determined by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz when irradiated with active energy rays having a wavelength of 365 nm at an integrated light intensity of 2000 to 4000 mJ / cm. 2The pressure-sensitive adhesive sheet according to

[15] or

[16] , wherein the shear storage modulus (G1'(85°C)) at a temperature of 85°C, as obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz when irradiated so as to satisfy the above condition, is 10 kPa or more.

[18] The pressure-sensitive adhesive sheet according to any of [1] to

[17] , wherein the gel fraction is 30 to 90%.

[19] The pressure-sensitive adhesive sheet according to any of [1] to

[18] , wherein the pressure-sensitive adhesive composition or syrup composition contains a crosslinking agent (B) and / or a photoinitiator (C).

[20] The pressure-sensitive adhesive sheet according to any of [1] to

[19] , wherein the pressure-sensitive adhesive composition or syrup composition contains a photoinitiator (C), wherein the photoinitiator (C) comprises a photoinitiator (c1) having, in its molecule, a radical-polymerizable functional group having a carbon-carbon double bond and a structure capable of generating a radical, and a hydrogen-abstraction photoinitiator (c2) other than the photoinitiator (c1).

[21] The pressure-sensitive adhesive sheet according to any one of [1] and [3] to

[20] , wherein the acrylic polymer (A) has a structural unit derived from a nitrogen-containing monomer (a3).

[22] A pressure-sensitive adhesive sheet with a release film, comprising the pressure-sensitive adhesive sheet according to any one of [1] to

[21] and a release film laminated on the pressure-sensitive adhesive sheet.

[23] A laminate for an image display device, comprising two image display device components and the pressure-sensitive adhesive sheet according to any one of [1] to

[21] interposed between the two image display device components, wherein one of the two image display device components is a surface protection panel and the other is a member consisting of any one or a combination of two or more selected from the group consisting of a touch sensor film, an image display panel, a color filter, a polarizing element, and a retardation film.

[24] The laminate for an image display device according to

[23] , wherein the surface protection panel has a frame-shaped concealing portion on the periphery, and the frame has a portion with a width of 3 mm or less.

[25] The laminate for an image display device according to

[23] or

[24] , which is fixed in a curved state.

[26] An image display device comprising the laminate for an image display device according to any one of

[23] to

[25] .

[27] A pressure-sensitive adhesive sheet for a component of an image display device, comprising the pressure-sensitive adhesive sheet according to any one of [1] to

[21] .

[0011] The pressure-sensitive adhesive sheet of the present invention can be attached without bubbles even to the peripheral edge near the edge of the pressure-sensitive adhesive sheet, which in conventional cases was located directly below the concealing portion and was therefore not visible. Therefore, the pressure-sensitive adhesive sheet can be suitably used as a pressure-sensitive adhesive sheet for image display devices, particularly image display devices with narrow frame designs or frameless designs.

[0012] An example of an embodiment of the present invention will be described in detail below. However, the present invention is not limited to the embodiment described below. In this specification, the term "film" conceptually includes a sheet, a film, and a tape. Furthermore, when the term "panel" is used, such as an image display panel or a protective panel, it includes a plate, a sheet, and a film.

[0013] In this specification, when it is stated that "x to y" (x and y are any numbers), it means "x or more and y or less" unless otherwise specified, and also includes the meaning of "preferably greater than x" or "preferably smaller than y." Furthermore, when it is stated that "x or more" (x is any number), it also includes the meaning of "preferably greater than x" unless otherwise specified, and when it is stated that "y or less" (y is any number), it also includes the meaning of "preferably smaller than y" unless otherwise specified. Furthermore, "x and / or y (x and y are any configurations)" means at least one of x and y, and can mean three possibilities: x only, y only, or x and y. Furthermore, in this specification, "(meth)acrylic" means a comprehensive definition of acrylic and methacrylic, "(meth)acrylate" means a comprehensive definition of acrylate and methacrylate, and "(meth)acryloyl" means a comprehensive definition of acryloyl and methacryloyl. Furthermore, in this specification, the term "major component" refers to a component that has a significant effect on the properties of the material, and the content of that component is usually 50% by mass or more, preferably 70% by mass or more, and particularly preferably 90% by mass or more, of the entire material. Furthermore, with regard to the numerical ranges described in stages in this specification, the upper or lower limit of a certain numerical range can be arbitrarily combined with the upper or lower limit of another numerical range. Furthermore, in the numerical ranges described in this specification, the upper or lower limit of the numerical range can also be replaced with the values ​​shown in the examples.

[0014] <<Adhesive Sheet>> A pressure-sensitive adhesive sheet according to one example of the first embodiment of the present invention (hereinafter referred to as "the present pressure-sensitive adhesive sheet 1") is a pressure-sensitive adhesive sheet having an acrylic pressure-sensitive adhesive layer formed from a pressure-sensitive adhesive composition containing an acrylic polymer (A), wherein the acrylic pressure-sensitive adhesive layer has a stress relaxation modulus (X0) of 0.20 or less, as calculated by the following formula (I) from the initial elastic modulus (G0'(0)) 0.1 second after applying a 25% strain at a temperature of 70°C to the acrylic pressure-sensitive adhesive layer and the relaxation modulus (G0'(300)) 300 seconds after applying a 25% strain at a temperature of 70°C: Stress relaxation rate (X0)=(G0'(300) / G0'(0)) (I) A pressure-sensitive adhesive sheet according to one example of the second embodiment of the present invention (hereinafter referred to as "the pressure-sensitive adhesive sheet 2") is a pressure-sensitive adhesive sheet having an acrylic pressure-sensitive adhesive layer, wherein the acrylic pressure-sensitive adhesive layer is a cured reaction product formed from a syrup composition comprising an alkyl (meth)acrylate (a1) having an alkyl group with 3 or more carbon atoms, and a hydroxyl group-containing (meth)acrylate (a2) and / or a nitrogen-containing monomer (a3), and wherein the stress relaxation rate (X0) calculated by the following formula (I) from the initial elastic modulus (G0'(0)) 0.1 second after applying a 25% strain at a temperature of 70°C to the acrylic pressure-sensitive adhesive layer and the relaxed elastic modulus (G0'(300)) 300 seconds after applying a 25% strain at a temperature of 70°C to the acrylic pressure-sensitive adhesive layer is 0.20 or less. Stress relaxation rate (X0)=(G0'(300) / G0'(0)) (I) Hereinafter, the present adhesive sheet 1 and the present adhesive sheet 2 (hereinafter sometimes referred to as "the present adhesive sheets 1 and 2") will be described.

[0015] The present pressure-sensitive adhesive sheets 1 and 2 satisfy the following requirement (1): Requirement (1) The stress relaxation rate (X0) calculated from the initial elastic modulus (G0'(0)) 0.1 seconds after applying a 25% strain at 70°C to the acrylic pressure-sensitive adhesive layer and the relaxation elastic modulus (G0'(300)) 300 seconds after applying a 25% strain at 70°C using the following formula (I) is 0.20 or less: Stress relaxation rate (X0) = (G0'(300) / G0'(0)) (I)

[0016] The present pressure-sensitive adhesive sheets 1 and 2, which satisfy requirement (1), have excellent stress relaxation properties, i.e., flexibility, and therefore are excellent at capturing foreign matter and defects that can be the starting point for foaming, and also easily diffuse air captured during lamination of components, thereby reducing or eliminating air bubbles remaining at the peripheral edge of the pressure-sensitive adhesive sheet.

[0017] In laminates requiring precision lamination, such as laminates for image display devices, finishing lamination is typically performed by heating and pressurizing using an autoclave when laminating components. After the autoclave process is completed or after the product begins to be used, air bubbles may form at the peripheral edges. One of the main causes of these bubbles is thought to be the infiltration of air present in the autoclave oven between the laminating components and the pressure-sensitive adhesive sheet due to the high pressure inside the oven during the lamination process. Conventionally, these air bubbles were not visible because the peripheral edges of displays were covered by a concealing layer such as a printed layer or a bezel. However, in recent years, due to demands for narrower display frames and frameless designs, the peripheral edges have become narrower, and there is a strong demand for improved bubble resistance at the peripheral edges of pressure-sensitive adhesive sheets.

[0018] From the viewpoint of improving the foaming resistance at the peripheral edge of the pressure-sensitive adhesive sheet, the stress relaxation rate (X0) is preferably 0.15 or less, more preferably 0.1 or less, and even more preferably 0.05 or less. On the other hand, from the viewpoint of suppressing adhesive extrusion, the stress relaxation rate (X0) is preferably 0.01 or more, more preferably 0.02 or more, even more preferably 0.03 or more, particularly preferably 0.04 or more, and most preferably 0.10 or more. The lower limit and upper limit of the stress relaxation rate (X0) can be arbitrarily combined.

[0019] The stress relaxation rate (X0) is determined as follows: the initial elastic modulus (G0'(0)) and the relaxation elastic modulus (G0'(300)) are measured by the method described below, and the obtained values ​​are substituted into the following formula (I) to calculate the stress relaxation rate (X0): Stress relaxation rate (X0) = (G0'(300) / G0'(0)) (I)

[0020] Examples of methods for adjusting the stress relaxation rate (X0) include, but are not limited to, methods for adjusting the composition and molecular weight of the acrylic polymer (A), the type and content of the crosslinking agent (B) and the photoinitiator (C), and methods for adjusting the amount of active energy ray irradiation.

[0021] It is preferable that the present pressure-sensitive adhesive sheets 1 and 2 further satisfy the following requirement (2): Requirement (2) The initial elastic modulus (G0'(0)) of the acrylic pressure-sensitive adhesive layer 0.1 seconds after applying a 25% strain at a temperature of 70°C is 5 to 100 kPa.

[0022] A pressure-sensitive adhesive sheet satisfying requirement (2) has a moderate cohesive force, and therefore is easy to handle. Furthermore, when the pressure-sensitive adhesive sheet is attached to a member, the peripheral edges of the pressure-sensitive adhesive sheet are less likely to be crushed, and adhesive extrusion at the edges can be reduced or eliminated. From the viewpoint of reducing adhesive extrusion, the initial modulus of elasticity (G0'(0)) is preferably 10 kPa or more, more preferably 15 kPa or more, and even more preferably 20 kPa or more. Furthermore, when the adherend has irregularities, from the viewpoint of filling in the surface irregularities during attachment, the initial modulus of elasticity (G0'(0)) is preferably 60 kPa or less, more preferably 50 kPa or less, and even more preferably 40 kPa or less. The lower and upper limits of the initial modulus of elasticity (G0'(0)) can be arbitrarily combined.

[0023] The initial elastic modulus (G0'(0)) is measured, for example, as follows: PSA sheets are repeatedly laminated to a thickness of 0.7 to 1.2 mm (for example, about 0.8 mm), and then punched out to a diameter of 8 mm. A strain of 25% is applied to the obtained sample at 70°C using a rheometer, and the elastic modulus is read after 0.1 seconds.

[0024] In measuring the initial modulus of elasticity (G0'(0)), it is necessary to avoid fluctuations in the measurement results due to the influence of the measuring jig. The initial modulus of elasticity (G0'(0)) is a value measured after adjusting the thickness to a range of 0.7 to 1.2 mm, which allows the initial modulus of elasticity (G0'(0)) to be accurately measured without being affected by the measuring jig. Note that "adjusted to a thickness of 0.7 to 1.2 mm" means that if the thickness of the pressure-sensitive adhesive sheet used as the measurement sample does not fall within this range, the thickness of the measurement sample is adjusted to fall within this range by, for example, stacking several sheets. The same applies when the thickness of the measurement sample is specified in other tests.

[0025] Examples of methods for adjusting the initial elastic modulus (G0'(0)) include a method of adjusting the composition or molecular weight of the acrylic polymer (A) or the type or amount of the crosslinking agent (B) or the photoinitiator (C), as well as a method of adjusting the amount of active energy ray irradiation. However, the methods are not limited to these.

[0026] It is preferable that the pressure-sensitive adhesive sheets 1 and 2 further satisfy the following requirement (3): Requirement (3) The acrylic pressure-sensitive adhesive layer has a relaxation modulus (G0'(300)) of 0.1 to 20 kPa 300 seconds after a 25% strain is applied at 70°C.

[0027] A pressure-sensitive adhesive sheet that satisfies requirement (3) has an appropriate cohesive strength, and therefore has excellent handleability. Furthermore, when attached to a member, the peripheral edge of the pressure-sensitive adhesive sheet is less likely to be crushed, and adhesive extrusion at the edge tends to be reduced or eliminated. From the viewpoint of reducing adhesive extrusion, the relaxation modulus (G0'(300)) is preferably 0.2 kPa or more, more preferably 0.5 kPa or more, and even more preferably 1 kPa or more. Furthermore, from the viewpoint of maintaining appropriate flexibility and ensuring wettability to the adherend, the relaxation modulus (G0'(300)) is preferably 15 kPa or less, more preferably 10 kPa or less, and even more preferably 5 kPa or less. The lower and upper limits of the relaxation modulus (G0'(300)) can be arbitrarily combined.

[0028] The relaxation modulus (G0'(300)) is measured, for example, as follows: PSA sheets are repeatedly laminated to a thickness of 0.7 to 1.2 mm (for example, about 0.8 mm), and then punched out to a diameter of 8 mm. A strain of 25% is applied to the obtained sample at 70°C using a rheometer, and the modulus is read after 300 seconds.

[0029] Examples of methods for adjusting the relaxation modulus (G0'(300)) include a method for adjusting the composition or molecular weight of the acrylic polymer (A) or the type or content of the crosslinking agent (B) or the photoinitiator (C), as well as a method for adjusting the amount of active energy ray irradiation. However, the methods are not limited to these.

[0030] It is preferable that the present PSA sheets 1 and 2 further satisfy the following requirement (4): Requirement (4) The shear storage modulus (G0'(25°C)) at 25°C, obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz, is 100 kPa or more.

[0031] PSA sheets that satisfy requirement (4) tend to have excellent handleability and resistance to adhesive extrusion. From this perspective, the shear storage modulus at 25°C (G0'(25°C)) is preferably 120 kPa or more, more preferably 150 kPa or more, even more preferably 200 kPa or more, particularly preferably 250 kPa or more, and of these, 300 kPa or more is preferred, and 400 kPa or more is most preferred. On the other hand, from the perspective of ensuring the stress relaxation properties of the PSA sheet, the shear storage modulus at 25°C (G0'(25°C)) is preferably 1000 kPa or less, more preferably 900 kPa or less, even more preferably 750 kPa or less, and particularly preferably 500 kPa or less. The lower limit and upper limit of the shear storage modulus at 25°C (G0'(25°C)) can be combined in any desired manner.

[0032] The shear storage modulus at 25°C (G0'(25°C)) is measured, for example, as follows. Pressure-sensitive adhesive sheets are repeatedly laminated to adjust the thickness to 0.7 to 1.2 mm (for example, 0.8 mm), and then punched out to a diameter of 8 mm. The obtained sample is subjected to dynamic viscoelasticity measurement using a rheometer under the conditions of a measurement jig: 8 mm diameter parallel plates, a frequency: 1 Hz, a measurement temperature: -50 to 150°C, and a heating rate: 5°C / min, and the value of the shear storage modulus at 25°C (G0'(25°C)) is read.

[0033] Examples of a method for adjusting the shear storage modulus at 25°C (G'(25°C)) within the above range include a method for adjusting the composition or molecular weight of the acrylic polymer (A) or the type or content of the crosslinking agent (B) or the photoinitiator (C), as well as a method for adjusting the amount of active energy ray irradiation. However, the method is not limited to these methods.

[0034] It is preferable that the pressure-sensitive adhesive sheets 1 and 2 further satisfy the following requirement (5): Requirement (5) The glass transition temperature (Tg0) defined as the maximum value of Tan δ obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz is −25° C. or higher.

[0035] PSA sheets that satisfy requirement (5) tend to have excellent handleability and resistance to adhesive extrusion. From this viewpoint, the glass transition temperature (Tg0) is preferably -20°C or higher, more preferably -15°C or higher, even more preferably -10°C or higher, particularly preferably -5°C or higher, and most preferably 0°C or higher. On the other hand, from the viewpoint of obtaining appropriate flexibility and stress relaxation, the upper limit is preferably 60°C or lower, more preferably 50°C or lower, even more preferably 40°C or lower, particularly preferably 20°C or lower, and of these, 5°C or lower is preferred. The lower limit and upper limit of the glass transition temperature (Tg0) can be combined arbitrarily.

[0036] The glass transition temperature (Tg) can be obtained by reading the temperature at which the loss tangent (Tan δ) becomes maximum, i.e., the peak temperature, from the dynamic viscoelastic spectrum data in shear mode obtained by the same measurement method as for the shear storage modulus (G'(25°C)) at 25°C described above. When there are multiple maximum values ​​in the viscoelastic spectrum, the "peak temperature" refers to the temperature at which the largest maximum value is obtained.

[0037] Examples of methods for adjusting the glass transition temperature (Tg0) within the above range include, but are not limited to, a method of adjusting the composition or molecular weight of the acrylic polymer (A) or the type or content of the crosslinking agent (B) or the photoinitiator (C), and a method of adjusting the amount of active energy ray irradiation.

[0038] It is preferable that the present pressure-sensitive adhesive sheets 1 and 2 further satisfy the following requirement (6): Requirement (6) The gel fraction of the pressure-sensitive adhesive sheet is 30 to 90%.

[0039] A pressure-sensitive adhesive sheet satisfying requirement (6) has a moderate cohesive strength and tends to have excellent handleability and shape stability. From the viewpoint of obtaining a moderate cohesive strength, the gel fraction is preferably 35% or more, more preferably 40% or more, and even more preferably 45% or more. On the other hand, from the viewpoint of obtaining stress relaxation, the gel fraction is preferably 90% or less, more preferably 87% or less, and even more preferably 85% or less. The lower limit and upper limit of the gel fraction can be arbitrarily combined.

[0040] The gel fraction is measured, for example, as follows: A pre-measured mass of the pressure-sensitive adhesive sheet and a 150-mesh SUS wire mesh are prepared. The pressure-sensitive adhesive sheet is then wrapped in the SUS wire mesh and immersed in ethyl acetate at 23°C for 24 hours. The sheet is then dried at 70°C for 4.5 hours, and the mass of the sheet and the SUS wire mesh is measured. The mass of the insoluble pressure-sensitive adhesive sheet remaining in the wire mesh (mass after immersion) is determined by subtracting the mass of the SUS wire mesh from the mass of the pressure-sensitive adhesive sheet before immersion in ethyl acetate (mass before immersion). The gel fraction (%) is then calculated as the percentage of the mass of the insoluble pressure-sensitive adhesive sheet remaining in the wire mesh (mass after immersion) relative to the mass of the pressure-sensitive adhesive sheet before immersion in ethyl acetate (mass before immersion).

[0041] Examples of methods for adjusting the gel fraction within the above range include, but are not limited to, a method of adjusting the composition or molecular weight of the acrylic polymer (A) or the type or content of the crosslinking agent (B) or the photoinitiator (C), and a method of adjusting the amount of active energy ray irradiation.

[0042] It is preferable that the present pressure-sensitive adhesive sheets 1 and 2 further satisfy the following requirement (7): Requirement (7) The adhesive strength of the acrylic pressure-sensitive adhesive layer to soda-lime glass at a temperature of 23° C. and a peeling rate of 60 mm / min is 2 N / cm or more.

[0043] An adhesive strength of 2 N / cm or more prevents peeling of the adhesive sheet edge surface, and excellent bonding reliability can be obtained at the peripheral edge. From this viewpoint, the adhesive strength is preferably 4 N / cm or more, more preferably 6 N / cm or more, and even more preferably 12 N / cm or more. The upper limit of the adhesive strength is not particularly limited, but from the viewpoint of reworkability, it is usually 50 N / cm, preferably 30 N / cm.

[0044] The adhesive strength is measured, for example, as follows. A 100 μm-thick polyethylene terephthalate (PET) film and an acrylic adhesive layer of an adhesive sheet are laminated together, and the other surface is roll-pressed onto soda-lime glass to obtain a laminated product. The laminated product is then autoclaved (temperature 60°C, gauge pressure 0.2 MPa, 20 minutes) to obtain a finished laminated product, which is used to measure adhesive strength. This sample is used to peel the film at a peel angle of 180° and a peel rate of 60 mm / min under an environment of 23°C and 50% RH, and the peel strength (N / cm) is determined as the adhesive strength.

[0045] The present pressure-sensitive adhesive sheets 1 and 2 are preferably active energy ray-curable. Here, the term "active energy ray-curable" means that the pressure-sensitive adhesive sheet has the property of being curable by active energy rays, in other words, that there is room for curing by active energy rays.

[0046] The present pressure-sensitive adhesive sheet 1 may be cured to a state where there is still room for curing by active energy rays (hereinafter also referred to as "primary curing"), or may be uncured (hereinafter also referred to as "uncured") and capable of being cured by active energy rays. Furthermore, the present pressure-sensitive adhesive sheet 2 is preferably primary cured. The primary cured or uncured pressure-sensitive adhesive sheet can be cured (hereinafter also referred to as "secondary curing") by irradiating it with active energy rays after being attached to an adherend.

[0047] When the present pressure-sensitive adhesive sheets 1 and 2 are actinic ray-curable, they preferably satisfy the following requirements.

[0048] Requirement (8) The adhesive sheet is exposed to active energy rays with a wavelength of 365 nm with an integrated light intensity of 2000 to 4000 mJ / cm 2 When the acrylic pressure-sensitive adhesive layer is irradiated so as to satisfy the above condition, the post-cure stress relaxation rate (X1) is calculated from the initial elastic modulus (G1'(0)) 0.1 seconds after applying a 25% strain at a temperature of 70°C and the relaxation elastic modulus (G1'(300)) 300 seconds after applying a 25% strain at a temperature of 70°C by the following formula (II), and is 0.22 or more. Post-cure stress relaxation rate (X1)=(G1'(300) / G1'(0)) (II)

[0049] A pressure-sensitive adhesive sheet that satisfies requirement (8) has excellent deformation resistance, and therefore tends to be less susceptible to dents or indentations when formed into a laminate for an image display device, and to exhibit excellent durability. From the viewpoint of obtaining excellent durability, the post-cure stress relaxation rate (X1) is preferably 0.25 or more, more preferably 0.30 or more, and even more preferably 0.35 or more. On the other hand, from the viewpoint of obtaining stress relaxation properties, the post-cure stress relaxation rate (X1) is preferably 1.00 or less, more preferably 0.80 or less, and even more preferably 0.70 or less. The lower limit and upper limit of the post-cure stress relaxation rate (X1) can be arbitrarily combined.

[0050] Requirement (9) The adhesive sheet is exposed to active energy rays with a wavelength of 365 nm with an integrated light intensity of 2000 to 4000 mJ / cm 2When irradiated so as to satisfy the above condition, the acrylic pressure-sensitive adhesive layer has an initial post-curing elastic modulus (G1'(0)) of 10 kPa or more 0.1 seconds after application of a 25% strain at a temperature of 70°C.

[0051] A pressure-sensitive adhesive sheet satisfying requirement (9) has high cohesive strength, and therefore tends to exhibit excellent durability against dents and indentations when formed into a laminate for an image display device. From the viewpoint of obtaining excellent durability, the initial elastic modulus after curing (G1'(0)) is preferably 15 kPa or more, more preferably 20 kPa or more, and even more preferably 25 kPa or more. On the other hand, from the viewpoint of obtaining stress relaxation properties, the initial elastic modulus after curing (G1'(0)) is preferably 200 kPa or less, more preferably 100 kPa or less, even more preferably 70 kPa or less, and particularly preferably 35 kPa or less. The lower limit and upper limit of the initial elastic modulus after curing (G1'(0)) can be arbitrarily combined. The method for measuring the initial elastic modulus after curing (G1'(0)) is the same as that for the initial elastic modulus (G0'(0)).

[0052] Requirement (10) The adhesive sheet is exposed to active energy rays with a wavelength of 365 nm with an integrated light intensity of 2000 to 4000 mJ / cm 2 When the acrylic pressure-sensitive adhesive layer is irradiated so as to satisfy the above condition, the acrylic pressure-sensitive adhesive layer has a post-cure relaxation modulus (G1'(300)) of 1 to 200 kPa after 300 seconds from application of a 25% strain at a temperature of 70°C.

[0053] A pressure-sensitive adhesive sheet satisfying requirement (10) has high cohesive strength, and therefore tends to exhibit excellent durability against dents and indentations when formed into a laminate for an image display device. From the viewpoint of obtaining excellent durability, the post-cure relaxation modulus (G1'(300)) is preferably 2 kPa or more, more preferably 3 kPa or more, even more preferably 5 kPa or more, and particularly preferably 8 kPa or more. On the other hand, from the viewpoint of obtaining stress relaxation properties, the post-cure relaxation modulus is preferably 200 kPa or less, more preferably 100 kPa or less, even more preferably 50 kPa or less, particularly preferably 20 kPa or less, and even more preferably 15 kPa or less, and most preferably 10 kPa or less. The lower limit and upper limit of the post-cure relaxation modulus (G1'(300)) can be arbitrarily combined. The method for measuring the post-cure relaxation modulus (G1'(300)) is the same as that for measuring the relaxation modulus (G0'(300)).

[0054] Requirement (11): The difference (X1-X0) between the post-cure stress relaxation rate (X1) and the stress relaxation rate (X0) is 0.01 or more.

[0055] A pressure-sensitive adhesive sheet that satisfies requirement (11) tends to be able to provide a laminate for image display with high levels of resistance to foaming at the peripheral edge and durability against dents and indentations. From this perspective, the value of requirement (11) is preferably 0.02 or more, more preferably 0.10 or more, and even more preferably 0.20 or more.

[0056] Requirement (12) The adhesive sheet is exposed to active energy rays with a wavelength of 365 nm with an integrated light intensity of 2000 to 4000 mJ / cm 2 When irradiated so as to satisfy the above condition, the shear storage modulus (G1'(25°C)) at 25°C after curing is 100 kPa or more, as determined by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz.

[0057] A pressure-sensitive adhesive sheet that satisfies requirement (12) tends to have high cohesive strength after exposure to active energy rays. From the viewpoint of obtaining high cohesive strength, the shear storage modulus at 25°C after curing (G1'(25°C)) is preferably 120 kPa or more, more preferably 150 kPa or more, even more preferably 200 kPa or more, and particularly preferably 400 kPa or more. On the other hand, from the viewpoint of obtaining stress relaxation properties, the shear storage modulus at 25°C after curing (G1'(25°C)) is preferably 1000 kPa or less, more preferably 900 kPa or less, even more preferably 800 kPa or less, particularly preferably 750 kPa or less, and most preferably 500 kPa or less. The lower limit and upper limit of the shear storage modulus at 25°C after curing (G1'(25°C)) can be arbitrarily combined. The shear storage modulus at 25°C after curing (G1'(25°C)) is measured in the same manner as the shear storage modulus at 25°C (G0'(25°C)).

[0058] Requirement (13) The adhesive sheet is exposed to active energy rays with a wavelength of 365 nm with an integrated light intensity of 2000 to 4000 mJ / cm 2 When the composition is irradiated so as to satisfy the above condition, the glass transition temperature (Tg1) after curing, which is defined as the maximum value of Tan δ obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz, is −25° C. or higher.

[0059] A pressure-sensitive adhesive sheet that satisfies requirement (13) tends to have high cohesive strength after exposure to active energy rays. From the viewpoint of obtaining high cohesive strength, the glass transition temperature (Tg1) after curing is preferably −23° C. or higher, more preferably −20° C. or higher, even more preferably −10° C. or higher, particularly preferably −5° C. or higher, and most preferably 0° C. or higher. On the other hand, from the viewpoint of obtaining stress relaxation properties, the glass transition temperature (Tg1) after curing is preferably 60° C. or lower, more preferably 40° C. or lower, even more preferably 30° C. or lower, and even more preferably 20° C. or lower, particularly preferably 5° C. or lower. The lower limit and upper limit of the glass transition temperature (Tg1) can be arbitrarily combined.

[0060] The method for measuring the glass transition temperature (Tg1) after curing is the same as that for measuring the glass transition temperature (Tg0).

[0061] Requirement (14) The adhesive sheet is exposed to active energy rays with a wavelength of 365 nm with an integrated light intensity of 2000 to 4000 mJ / cm 2 When irradiated so as to achieve this, the gel fraction of the pressure-sensitive adhesive sheet (gel fraction after curing) is 35 to 95%.

[0062] A pressure-sensitive adhesive sheet that satisfies requirement (14) has high cohesive strength and can exhibit excellent durability when formed into a laminate for an image display device. From the viewpoint of obtaining excellent durability, the gel fraction after curing is preferably 40% or more, more preferably 45% or more, and even more preferably 50% or more. On the other hand, from the viewpoint of obtaining appropriate stress relaxation, the gel fraction after curing is preferably 95% or less, more preferably 90% or less. The lower limit and upper limit of the gel fraction after curing can be arbitrarily combined.

[0063] The method for measuring the gel fraction after curing is the same as that for measuring the gel fraction.

[0064] Requirement (15) The adhesive sheet is exposed to active energy rays with a wavelength of 365 nm with an integrated light intensity of 2000 to 4000 mJ / cm 2 When irradiated so as to satisfy the above condition, the adhesive strength of the acrylic adhesive layer after curing to soda lime glass at a temperature of 23° C. and a peeling rate of 60 mm / min is 2 N / cm or more.

[0065] A pressure-sensitive adhesive sheet that satisfies requirement (15) tends to exhibit excellent reliability without peeling even when used as a laminate for an image display device. From this viewpoint, the adhesive strength after curing is preferably 3 N / cm or more, more preferably 8 N / cm or more, and even more preferably 12 N / cm or more. The upper limit of the adhesive strength after curing is not particularly limited, but from the viewpoint of reworkability, it is usually 50 N / cm, preferably 30 N / cm.

[0066] The adhesive strength after curing is measured, for example, as follows: A 100 μm thick polyethylene terephthalate (PET) film as a backing film is laminated to the acrylic adhesive layer of the adhesive sheet, and the other side is roll-pressed onto soda lime glass, followed by autoclaving (temperature 60°C, gauge pressure 0.2 MPa, 20 minutes) for finish lamination. Thereafter, the integrated light intensity at a wavelength of 365 nm is measured to be 2000 to 4000 mJ / cm. 2 The adhesive sheet is cured by irradiating the adhesive sheet with active energy rays through the backing film to obtain a sample for measuring adhesive strength. The adhesive strength after curing is determined by peeling this sample at a peel angle of 180° and a peel rate of 60 mm / min under an environment of 23°C and 50% RH.

[0067] <Present Pressure-Sensitive Adhesive Sheet 1> The present pressure-sensitive adhesive sheet 1 has an acrylic pressure-sensitive adhesive layer formed from a pressure-sensitive adhesive composition containing an acrylic polymer (A). Preferably, the pressure-sensitive adhesive composition further contains a crosslinking agent (B) and a photoinitiator (C). Furthermore, the pressure-sensitive adhesive composition may further contain other components in addition to the acrylic polymer (A), the crosslinking agent (B), and the photoinitiator (C). When the pressure-sensitive adhesive composition is active energy ray-curable, the present pressure-sensitive adhesive sheet 1 is typically obtained by curing a pressure-sensitive adhesive composition containing the acrylic polymer (A). Each component contained in the pressure-sensitive adhesive composition will be described in detail below.

[0068] [Acrylic Polymer (A)] Examples of the acrylic polymer (A) include a homopolymer of alkyl(meth)acrylate, as well as a copolymer obtained by polymerizing a monomer component copolymerizable therewith. Among these, it is preferable that the acrylic polymer (A) contains two or more copolymerization components, and at least one of the copolymerization components is an alkyl(meth)acrylate (a1) having an alkyl group with 3 to 30 carbon atoms (hereinafter, sometimes referred to as "alkyl(meth)acrylate (a1)").

[0069] A more specific example of the acrylic polymer (A) is a copolymer of copolymerization components containing an alkyl(meth)acrylate (a1) and at least one copolymerizable monomer selected from the group consisting of alkyl(meth)acrylate (a1), a hydroxyl group-containing monomer (a2), a nitrogen-containing monomer (a3), a carboxy group-containing monomer (a4), an epoxy group-containing monomer (a5), a vinyl monomer (a6), an alkyl(meth)acrylate monomer (a7) having an alkyl group with 1 or 2 carbon atoms, an alicyclic monomer (a8), a macromonomer (a9), and other copolymerizable monomers (a10) [hereinafter, these may be referred to as "copolymerizable monomers (a2) to (a10)"]. Among these, the inclusion of a hydroxyl group-containing monomer (a2) and / or a nitrogen-containing monomer (a3) ​​as the copolymerization component is preferred in that it allows for corrosion resistance, adhesion, and resistance to wet heat whitening when the adherend contains a corrosive component such as a metal, and the inclusion of a hydroxyl group-containing monomer (a2) and a nitrogen-containing monomer (a3) ​​is particularly preferred in that it further enhances cohesion. Furthermore, when the adherend contains a corrosive component such as a metal, it is preferable that the copolymerization component does not contain a carboxyl group-containing monomer (a4) in terms of corrosion resistance. Such an acrylic polymer (A) usually has structural units derived from the alkyl (meth)acrylate (a1) as well as structural units derived from the copolymerizable monomers (a2) to (a10) contained in the copolymerization component.

[0070] [Alkyl (meth)acrylate (a1)] The alkyl (meth)acrylate (a1) is a linear or branched alkyl (meth)acrylate having an alkyl group with 3 to 30 carbon atoms, and is represented by the following formula (Chemical Formula 1): CH═C(R 1 )-COO(R 2 )...(Chemical formula 1) (In Chemical formula 1, R 1 represents a hydrogen atom or a methyl group, R 2 represents a linear or branched alkyl group having 3 to 30 carbon atoms.

[0071] Examples of the alkyl(meth)acrylate represented by the formula (Chemical Formula 1) include linear alkyl(meth)acrylates such as n-propyl(meth)acrylate, i-propyl(meth)acrylate, n-butyl(meth)acrylate, n-pentyl(meth)acrylate, n-hexyl(meth)acrylate, n-heptyl(meth)acrylate, n-octyl(meth)acrylate, n-nonyl(meth)acrylate, n-decyl(meth)acrylate, undecyl(meth)acrylate, lauryl(meth)acrylate, n-tridecyl(meth)acrylate, n-tetradecyl(meth)acrylate, cetyl(meth)acrylate, stearyl(meth)acrylate, icosyl(meth)acrylate, henicosyl(meth)acrylate, and behenyl(meth)acrylate; sec-butyl(meth)acrylate; Examples of branched alkyl (meth)acrylates include isobutyl (meth)acrylate, t-butyl (meth)acrylate, isopentyl (meth)acrylate, neopentyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, isodecyl (meth)acrylate, isobornyl (meth)acrylate, isostearyl (meth)acrylate, isoicosyl (meth)acrylate, butyloctyl (meth)acrylate, isomyristyl (meth)acrylate, isocetyl (meth)acrylate, hexyldecyl (meth)acrylate, isostearyl (meth)acrylate, octyldecyl (meth)acrylate, octyldodecyl (meth)acrylate, and isobehenyl (meth)acrylate. These may be used alone or in combination of two or more.

[0072] Among these, linear alkyl (meth)acrylates are preferred from the viewpoint of obtaining flexibility. Furthermore, from the viewpoint of balancing adhesiveness and flexibility, linear alkyl (meth)acrylates having an alkyl group of 3 to 20 carbon atoms, more preferably 5 to 18, particularly 6 to 16, and even more particularly 7 to 14 carbon atoms are preferred, and examples thereof include n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, decyl (meth)acrylate, and lauryl (meth)acrylate.

[0073] Among these, branched-chain alkyl(meth)acrylates, i.e., alkyl(meth)acrylates containing a tertiary carbon atom in the alkyl group, are preferred because they facilitate the hydrogen abstraction reaction described below upon irradiation with active energy rays, thereby enabling efficient formation of a crosslinked structure. Among these, branched-chain alkyl(meth)acrylates in which the alkyl group contains 3 to 20 carbon atoms, more preferably 5 to 18, particularly 6 to 16, and even more particularly 7 to 14 carbon atoms, are preferred. For example, sec-butyl(meth)acrylate, isobutyl(meth)acrylate, t-butyl(meth)acrylate, isopentyl(meth)acrylate, neopentyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, isooctyl(meth)acrylate, isononyl(meth)acrylate, isodecyl(meth)acrylate, and isobornyl(meth)acrylate are preferred, with 2-ethylhexyl(meth)acrylate and isobornyl(meth)acrylate being particularly preferred.

[0074] The proportion of the alkyl (meth)acrylate (a1)-derived structural units relative to the acrylic polymer (A) is typically 5 to 95% by mass, preferably 10 to 90% by mass, more preferably 15 to 85% by mass, and particularly preferably 20 to 80% by mass. When the proportion of the alkyl (meth)acrylate (a1)-derived structural units is equal to or greater than the lower limit, the flexibility tends to be excellent, and when the adherend has irregularities, the conformability tends to be excellent. When the proportion is equal to or less than the upper limit, the effect of the copolymerizable monomer described below is easily obtained, and the adhesive strength and cohesive strength tend to be excellent.

[0075] [Hydroxyl Group-Containing Monomer (a2)] Examples of the hydroxyl group-containing monomer (a2) include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 5-hydroxypentyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and 8-hydroxyoctyl (meth)acrylate; caprolactone-modified hydroxy (meth)acrylates such as caprolactone-modified 2-hydroxyethyl (meth)acrylate; diethylene glycol (meth)acrylate; polyethylene glycol (meth)acrylate; polypropylene glycol (meth)acrylate; polytetramethylene glycol (meth)acrylate; polyoxyethylene poly(meth)acrylate; Examples of such monomers include (meth)acrylates having an oxyalkylene structure such as propylene glycol (meth)acrylate, primary hydroxyl group-containing (meth)acrylates such as 2-acryloyloxyethyl-2-hydroxyethyl phthalate, secondary hydroxyl group-containing (meth)acrylates such as 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, and 3-chloro-2-hydroxypropyl (meth)acrylate, tertiary hydroxyl group-containing (meth)acrylates such as 2,2-dimethyl 2-hydroxyethyl (meth)acrylate, and vinyl ethers such as 2-hydroxyethyl vinyl ether, diethylene glycol monovinyl ether, and 4-hydroxybutyl vinyl ether. These may be used alone or in combination of two or more. The hydroxyl group-containing monomer (a2) improves the adhesive strength of the pressure-sensitive adhesive sheet and can suppress whitening under heat and humidity. Furthermore, when the pressure-sensitive adhesive composition contains a thermal crosslinking agent, as described below, it serves as a crosslinking reaction site.

[0076] Among the hydroxyl group-containing monomers (a2), preferred are hydroxyl group-containing monomers having a hydroxyalkyl group having 1 to 10, more preferably 1 to 6, and even more preferably 2 to 4 carbon atoms, such as 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxyethyl vinyl ether, diethylene glycol monovinyl ether, and 4-hydroxybutyl vinyl ether, and particularly preferred are primary hydroxyl group-containing (meth)acrylates, such as 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate.

[0077] When the acrylic polymer (A) has a structural unit derived from a hydroxyl group-containing monomer (a2), the content thereof is usually 3 to 30 mass%, preferably 5 to 25 mass%, particularly preferably 7 to 20 mass%, based on the acrylic polymer (A), from the viewpoint of imparting adhesive strength and resistance to wet heat whitening.

[0078] [Nitrogen-Containing Monomer (a3)] Examples of the nitrogen-containing monomer (a3) ​​include amino group-containing monomers, amide group-containing monomers, isocyanate group-containing monomers, and (meth)acrylonitrile. These may be used alone or in combination of two or more. The nitrogen-containing monomer (a3) ​​improves the cohesive strength of the pressure-sensitive adhesive sheet and can suppress wet heat whitening. Furthermore, when a hydrogen abstraction photoinitiator described below is used, it is preferable that the acrylic polymer (A) has a structural unit derived from the nitrogen-containing monomer (a3). When a hydrogen abstraction photoinitiator described below is used, the nitrogen-containing monomer (a3) ​​has the effect of promoting the hydrogen abstraction reaction.

[0079] Examples of the amino group-containing monomer include primary amino group-containing (meth)acrylates such as aminomethyl (meth)acrylate and aminoethyl (meth)acrylate; secondary amino group-containing (meth)acrylates such as t-butylaminoethyl (meth)acrylate and t-butylaminopropyl (meth)acrylate; tertiary amino group-containing (meth)acrylates such as ethylaminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, diethylaminopropyl (meth)acrylate, and dimethylaminopropylacrylamide; and monomers such as N-vinylpyrrolidone, methylvinylpyrrolidone, vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole, vinylmorpholine, (meth)acryloylmorpholine, N-vinylacetamides, and N-vinylcaprolactam.

[0080] Examples of the amide group-containing monomer include (meth)acrylamide; N-alkyl(meth)acrylamides such as N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N-propyl(meth)acrylamide, N-n-butyl(meth)acrylamide, diacetone(meth)acrylamide, and N,N'-methylenebis(meth)acrylamide; N,N-dialkyl(meth)acrylamides such as N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropyl(meth)acrylamide, N,N-ethylmethylacrylamide, and N,N-diallyl(meth)acrylamide; hydroxyalkyl(meth)acrylamides such as N-hydroxymethyl(meth)acrylamide and N-hydroxyethyl(meth)acrylamide; alkoxyalkyl(meth)acrylamides such as N-methoxymethyl(meth)acrylamide and N-(n-butoxymethyl)(meth)acrylamide; maleimide or a derivative thereof. Among these, (meth)acrylamide is preferred.

[0081] Examples of the isocyanate group-containing monomer include 2-(meth)acryloyloxyethyl isocyanate and alkylene oxide adducts thereof, etc. The isocyanate group may be protected with a blocking agent such as methyl ethyl ketone oxime, 3,5-dimethylpyrazole, 1,2,4-triazole, or diethyl malonate.

[0082] Among these, those having a tertiary nitrogen atom are preferred, as they have a sensitizing effect on the hydrogen abstraction reaction by the hydrogen abstraction photoinitiator described below, and as a result, can efficiently form a crosslinked structure. Tertiary amino group-containing (meth)acrylates, N,N-dialkyl(meth)acrylamides, N-vinylpyrrolidone, acryloylmorpholine, and the like are particularly preferred.

[0083] When the acrylic polymer (A) has a structural unit derived from a nitrogen-containing monomer (a3), the content thereof is usually 0.1 to 15 mass%, preferably 0.5 to 13 mass%, particularly preferably 1 to 10 mass%, and especially preferably 2 to 7 mass%, relative to the acrylic polymer (A), from the viewpoint of imparting cohesive strength and resistance to wet heat whitening.

[0084] [Carboxy Group-Containing Monomer (a4)] Examples of the carboxy group-containing monomer (a4) include (meth)acrylic acid, 2-(meth)acryloyloxyethyl hexahydrophthalic acid, 2-(meth)acryloyloxypropyl hexahydrophthalic acid, 2-(meth)acryloyloxyethyl phthalic acid, 2-(meth)acryloyloxypropyl phthalic acid, 2-(meth)acryloyloxyethyl maleic acid, 2-(meth)acryloyloxypropyl maleic acid, 2-(meth)acryloyloxyethyl succinic acid, 2-(meth)acryloyloxypropyl succinic acid, crotonic acid, fumaric acid, maleic acid, itaconic acid, etc. These may be used alone or in combination of two or more.

[0085] When the acrylic polymer (A) has a structural unit derived from a carboxy group-containing monomer (a4), the content thereof is usually 0.1 to 15 mass%, preferably 0.3 to 13 mass%, more preferably 0.5 to 10 mass%, and particularly preferably 1 to 6 mass%, based on the acrylic polymer (A).

[0086] [Epoxy Group-Containing Monomer (a5)] Examples of the epoxy group-containing monomer (a5) include glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate glycidyl ether. These may be used alone or in combination of two or more.

[0087] When the acrylic polymer (A) has a structural unit derived from an epoxy group-containing monomer (a5), the content thereof is usually 0.1 to 15 mass%, preferably 0.3 to 13 mass%, more preferably 0.5 to 10 mass%, and particularly preferably 1 to 6 mass%, based on the acrylic polymer (A).

[0088] [Vinyl Monomer (a6)] Examples of the vinyl monomer (a6) include compounds having a vinyl group in the molecule. Examples of such compounds include vinyl ester monomers such as vinyl acetate, vinyl propionate, vinyl laurate, and vinyl stearate, as well as aromatic vinyl monomers such as styrene, chlorostyrene, chloromethylstyrene, α-methylstyrene, and other substituted styrenes. These may be used alone or in combination of two or more.

[0089] When the acrylic polymer (A) has a constituent moiety derived from a vinyl monomer (a3), the content thereof is usually 1 to 40 mass %, preferably 5 to 35 mass %, more preferably 8 to 30 mass %, and particularly preferably 10 to 25 mass %, relative to the acrylic polymer (A), from the viewpoint of imparting cohesive strength to the PSA sheet.

[0090] [Alkyl(meth)acrylate Monomer (a7) in Which the Alkyl Group Has 1 or 2 Carbon Atoms] Examples of the alkyl(meth)acrylate monomer (a7) in Which the alkyl group has 1 or 2 carbon atoms include methyl(meth)acrylate and ethyl(meth)acrylate. These may be used alone or in combination of two or more.

[0091] When the acrylic polymer (A) has a structural unit derived from an alkyl(meth)acrylate monomer (a7), the content thereof is, from the viewpoint of imparting cohesive strength to the PSA sheet, usually 1 to 60 mass%, preferably 5 to 55 mass%, particularly preferably 10 to 50 mass%, and especially preferably 15 to 45 mass%, relative to the acrylic polymer (A).

[0092] [Alicyclic Monomer (a8)] Examples of the alicyclic monomer (a8) include cyclohexyl (meth)acrylate, 3,3,5-trimethylcyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, adamantyl (meth)acrylate, etc. These may be used alone or in combination of two or more.

[0093] When the acrylic polymer (A) has a structural unit derived from an alicyclic monomer (a8), the content thereof is, from the viewpoint of imparting cohesive strength to the PSA sheet, usually 0.1 to 15 mass%, preferably 0.5 to 13 mass%, particularly preferably 1 to 10 mass%, and especially preferably 2 to 7 mass%, relative to the acrylic polymer (A).

[0094] [Macromonomer (a9)] The macromonomer (a9) is a monomer that, when polymerized into the acrylic polymer (A), can easily increase the number of carbon atoms in the side chain of the acrylic polymer (A), for example, to 20 or more. By using the macromonomer (a9) as a copolymerization component, the acrylic polymer (A) can be made into a graft copolymer having a constituent portion (segment) derived from the macromonomer (a9). Furthermore, by changing the blending ratio of the macromonomer (a9) to other monomers, the properties of the main chain and side chain of the graft copolymer can be changed.

[0095] The macromonomer (a9) has a radically polymerizable functional group or a functional group such as a hydroxy group, an isocyanate group, an epoxy group, a carboxy group, an amino group, an amide group, or a thiol group. The macromonomer (a9) may have these functional groups alone or in combination of two or more. Among these, the macromonomer (a9) preferably has a radically polymerizable functional group copolymerizable with other monomers. The macromonomer (a9) may contain one or more radically polymerizable functional groups, with one being particularly preferred. Furthermore, when the macromonomer (a9) has a functional group, the macromonomer may contain one or more functional groups, with one being particularly preferred.

[0096] The macromonomer (a9) preferably has a backbone component composed of an acrylic polymer or a vinyl polymer. Examples of backbone components of the macromonomer (a9) include alkyl(meth)acrylates (a1) in which the alkyl group has 3 to 30 carbon atoms, the vinyl monomers (a6), alkyl(meth)acrylate monomers (a7) in which the alkyl group has 1 or 2 carbon atoms, and alicyclic monomers (a8). These may be used alone or in combination of two or more. Among these, the use of alkyl(meth)acrylates or alicyclic monomers in which the alkyl group has 1 to 8 carbon atoms, or aromatic monomers such as styrene, as backbone components is preferred, as they can provide pressure-sensitive adhesive sheets with excellent cohesive strength. On the other hand, the use of alkyl(meth)acrylates in which the alkyl group has 9 to 30 carbon atoms is preferred, as they can provide pressure-sensitive adhesive sheets with excellent flexibility.

[0097] The number average molecular weight of the macromonomer (a9) is preferably from 1,000 to 40,000, more preferably from 1,500 to 20,000, and even more preferably from 2,000 to 15,000. The number average molecular weight of the macromonomer (a9) is a value measured by gel permeation chromatography (GPC) in terms of standard polystyrene.

[0098] As the macromonomer (a9), a generally produced macromonomer (for example, a macromonomer manufactured by Toagosei Co., Ltd.) can be used appropriately.

[0099] When the acrylic polymer (A) has a structural unit derived from macromonomer (a9), the content thereof is usually 1 to 30% by mass, preferably 3 to 20% by mass, and more preferably 5 to 18% by mass, relative to the acrylic polymer (A). If the content is equal to or greater than the lower limit, the phase separation force between the segment containing the structural unit derived from macromonomer (a9) and the segment formed by the other structural units becomes stronger, and the cohesive strength of the PSA sheet tends to be better. If the content is equal to or less than the upper limit, the phase-separated structure tends to collapse more easily during lamination, and the unevenness-following ability tends to be better.

[0100] [Other Copolymerizable Monomers (a10)] Examples of the other copolymerizable monomers (a10) include (meth)acrylates having an alkoxyalkylene glycol skeleton, such as methoxydiethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, butoxypolyethylene glycol (meth)acrylate, methoxypolypropylene glycol (meth)acrylate, butoxypolypropylene glycol (meth)acrylate, methoxypolytetramethylene glycol (meth)acrylate, butoxypolytetramethylene glycol (meth)acrylate, methoxypolyoxyethylene polyoxypropylene glycol (meth)acrylate, and butoxypolyoxyethylene polyoxypropylene glycol (meth)acrylate; phenyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenyldiethylene glycol (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, and phenoxypolyethylene glycol-polypropylene glycol-(meth)acrylate; aromatic (meth)acrylates such as acrylate and nonylphenol ethylene oxide adduct (meth)acrylate, 4-acryloyloxybenzophenone, 4-acryloyloxyethoxybenzophenone, 4-acryloyloxy-4'-methoxybenzophenone, 4-acryloyloxyethoxy-4'-methoxybenzophenone, 4-acryloyloxy-4'-bromobenzophenone, 4-acryloyloxyethoxy-4'-bromobenzophenone, 4-methacryloyloxybenzophenone, 4- Examples include (meth)acrylates having a benzophenone structure such as methacryloyloxyethoxybenzophenone, 4-methacryloyloxy-4'-methoxybenzophenone, 4-methacryloyloxyethoxy-4'-methoxybenzophenone, 4-methacryloyloxy-4'-bromobenzophenone, 4-methacryloyloxyethoxy-4'-bromobenzophenone, and mixtures thereof, heterocycle-containing (meth)acrylates such as tetrahydrofurfuryl (meth)acrylate, and macromonomers. These may be used alone or in combination of two or more.

[0101] When the acrylic polymer (A) has a structural unit derived from another copolymerizable monomer (a10), the content thereof is usually 1 to 30% by mass, preferably 3 to 20% by mass, and more preferably 5 to 15% by mass, based on the acrylic polymer (A).

[0102] The method for producing the acrylic polymer (A) is not particularly limited, and may be, for example, by polymerizing a copolymerization component containing an alkyl(meth)acrylate (a1) and, if necessary, at least one selected from the group consisting of copolymerizable monomers (a2) to (a10).

[0103] Examples of the polymerization method include conventionally known methods such as solution polymerization, suspension polymerization, bulk polymerization, and emulsion polymerization. Among these, solution polymerization is preferred in that it allows safe and stable production of an acrylic resin with any monomer composition. Thus, the acrylic polymer (A) can be obtained.

[0104] The acrylic polymer (A) may have a photoactive moiety, such as a polymerizable carbon-carbon double bond group, introduced into its side chain, thereby increasing the crosslinking efficiency of the pressure-sensitive adhesive composition and enabling the pressure-sensitive adhesive composition to be crosslinked in a shorter time, thereby increasing productivity.

[0105] Examples of a method for introducing a polymerizable carbon-carbon double bond group into the side chain of the acrylic polymer (A) include a method in which a copolymer containing a functional group-containing ethylenically unsaturated monomer such as the above-mentioned hydroxyl group-containing monomer (a2), nitrogen atom-containing monomer (a3), carboxy group-containing monomer (a4), or epoxy group-containing monomer (a5) is prepared, and then a compound having a polymerizable carbon-carbon double bond group and a functional group reactive with the functional group is subjected to a condensation or addition reaction while maintaining the activity of the polymerizable carbon-carbon double bond group.

[0106] Examples of combinations of these functional groups include an epoxy group (glycidyl group) and a carboxy group, an amino group and a carboxy group, an amino group and an isocyanate group, an epoxy group (glycidyl group) and an amino group, a hydroxyl group and an epoxy group, and a hydroxyl group and an isocyanate group. Among these combinations of functional groups, a combination of a hydroxyl group and an isocyanate group is preferred because of the ease of reaction control. Among these, a combination in which the copolymer has a hydroxyl group and the compound has an isocyanate group is preferred.

[0107] Examples of the isocyanate compound having a polymerizable carbon-carbon double bond group include the above-mentioned 2-(meth)acryloyloxyethyl isocyanate and alkylene oxide adducts thereof.

[0108] From the viewpoint of improving adhesiveness and stress relaxation properties, the content of the compound having a functional group reactive with the functional group and a polymerizable carbon-carbon double bond group is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, even more preferably 1 part by mass or less, and particularly preferably 0.1 parts by mass or less, relative to 100 parts by mass of the acrylic polymer (A). The lower limit is usually 0 part by mass.

[0109] The weight average molecular weight (Mw) of the acrylic polymer (A) is preferably 200,000 or more, more preferably 300,000 or more, and even more preferably 400,000 or more, from the viewpoint of obtaining a pressure-sensitive adhesive composition with high cohesive strength. Furthermore, the upper limit of the weight average molecular weight (Mw) of the acrylic polymer (A) is preferably 1.5 million or less, more preferably 1.2 million or less, even more preferably 1.1 million or less, and particularly preferably 1 million or less, from the viewpoint of ease of handling and uniform stirring. The lower and upper limits of the weight average molecular weight of the acrylic polymer (A) can be arbitrarily combined. The weight average molecular weight of the acrylic polymer (A) is a value calculated in terms of standard polystyrene measured by gel permeation chromatography (GPC).

[0110] The acrylic polymer (A) is preferably the main component of the pressure-sensitive adhesive composition. Here, "main component" refers to the component with the highest content among the components of the pressure-sensitive adhesive composition. Specifically, the content of the acrylic polymer (A) is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more, based on the total mass of the pressure-sensitive adhesive composition. The upper limit is 100% by mass, but is usually preferably 99% by mass or less, more preferably 98% by mass or less, and even more preferably 97% by mass or less.

[0111] [Crosslinking Agent (B)] The pressure-sensitive adhesive composition preferably contains a crosslinking agent (B) from the viewpoint of promoting the crosslinking reaction. This allows the pressure-sensitive adhesive composition to efficiently form a crosslinked structure. Furthermore, when a crosslinked structure is formed in a pressure-sensitive adhesive sheet using the pressure-sensitive adhesive composition, adhesive extrusion during storage or application can be prevented, and good adhesiveness and cohesive strength can be obtained. However, when the acrylic polymer (A) undergoes a hydrogen abstraction reaction due to the action of a photoinitiator (C) described below or the like, and a sufficient crosslinked structure can be formed within the acrylic polymer (A) and / or between the acrylic polymers (A), the crosslinking agent (B) does not necessarily need to be contained.

[0112] Examples of the crosslinking agent (B) include acrylic crosslinking agents, isocyanate crosslinking agents, epoxy crosslinking agents, aziridine crosslinking agents, melamine crosslinking agents, aldehyde crosslinking agents, amine crosslinking agents, and metal chelate crosslinking agents. Among these, isocyanate crosslinking agents are preferred because of their excellent reactivity with the acrylic polymer (A). On the other hand, acrylic crosslinking agents are preferred, and polyfunctional (meth)acrylates are particularly preferred, from the viewpoints of ease of reaction control and active energy ray curability.

[0113] Examples of the polyfunctional (meth)acrylate include polyfunctional (meth)acrylic monomers and polyfunctional (meth)acrylic oligomers having two or more (meth)acryloyl groups, which may be used alone or in combination of two or more.

[0114] Examples of the polyfunctional (meth)acrylic monomer include pentanediol di(meth)acrylate, hexadiol di(meth)acrylate, heptanediol di(meth)acrylate, octanediol di(meth)acrylate, nonanediol di(meth)acrylate, decanediol di(meth)acrylate, undecanediol di(meth)acrylate, dodecanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, glycerin di(meth)acrylate, neopentyl glycol di(meth)acrylate, glycerin glycidyl ether di(meth)acrylate, tricyclodecane dimethacrylate, tricyclodecane dimethanol di(meth)acrylate, bisphenol A polyethoxy di(meth)acrylate, bisphenol A polypropoxy di(meth)acrylate, bisphenol F polyethoxy di(meth)acrylate, ethylene glycol di(meth)acrylate tri(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane trioxyethyl (meth)acrylate, ε-caprolactone-modified tris(2-hydroxyethyl) isocyanurate tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propoxylated pentaerythritol tri(meth)acrylate, ethoxylated pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, propoxylated pentaerythritol tri(meth)acrylate Pentaerythritol tetra(meth)acrylate, ethoxylated pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, tris(acryloxyethyl)isocyanurate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol penta(meth)acrylate , tripentaerythritol hexa(meth)acrylate, tripentaerythritol penta(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, di(meth)acrylate of hydroxypivalic acid neopentyl glycol ε-caprolactone adduct, trimethylolpropane tri(meth)acrylate, trimethylolpropane polyethoxytri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, etc.

[0115] Examples of the polyfunctional (meth)acrylic oligomer include polyester (meth)acrylate oligomers, epoxy (meth)acrylate oligomers, urethane (meth)acrylate oligomers, and polyether (meth)acrylate oligomers.

[0116] Among these crosslinking agents (B), polyfunctional (meth)acrylate monomers and oligomers having a glycol structure are preferred from the viewpoint of imparting appropriate flexibility to the cured product, and acrylic acid adducts of pentaerythritol and dipentaerythritol, and alkoxylated products thereof are preferred from the viewpoint of imparting cohesive strength.

[0117] When the pressure-sensitive adhesive composition contains a crosslinking agent (B), the content thereof is usually 0.1 parts by mass or more, preferably 0.5 parts by mass or more, and more preferably 1 part by mass or more, per 100 parts by mass of the acrylic polymer (A), from the viewpoint of imparting shape stability to the pressure-sensitive adhesive sheet and durability when formed into a laminate for an image display device. Furthermore, the upper limit is usually 25 parts by mass or less, preferably 22 parts by mass or less, more preferably 20 parts by mass or less, and particularly preferably 18 parts by mass or less, from the viewpoint of maintaining the flexibility of the pressure-sensitive adhesive sheet. The lower and upper limits of the content of the crosslinking agent (B) can be arbitrarily combined.

[0118] [Photoinitiator (C)] The pressure-sensitive adhesive composition preferably contains a photoinitiator (C). The photoinitiator (C) is a compound that generates radicals when exposed to active energy rays. The photoinitiators (C) are broadly classified into two types based on the radical generation mechanism. More specifically, they are broadly classified into cleavage-type photoinitiators, which can generate radicals by cleaving and decomposing the single bond of the photoinitiator itself, and hydrogen-abstraction-type photoinitiators, which can generate radicals by the excited initiator abstracting hydrogen from a hydrogen donor in the system. These may be used alone or in combination of two or more types. The cleavage-type photoinitiator is preferred because it has high photosensitivity. On the other hand, the hydrogen-abstraction-type photoinitiator is preferred because it does not generate photodecomposition products and can incorporate the acrylic polymer (A) into a crosslinked structure through a hydrogen abstraction reaction.

[0119] Examples of the hydrogen abstraction photoinitiator include benzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, 4-phenylbenzophenone, 3,3'-dimethyl-4-methoxybenzophenone, methyl 2-benzoylbenzoate, 4-[(4-methylphenyl)thio]benzophenone, 4-acryloyloxybenzophenone, 4-acryloyloxyethoxybenzophenone, 4-acryloyloxy-4'-methoxybenzophenone, 4-acryloyloxyethoxy-4'-methoxybenzophenone, 4-acryloyloxy-4'-bromobenzophenone, 4-acryloyloxyethoxy-4'-bromobenzophenone, 4-methacryloyloxy-4'-bromobenzophenone, Examples of suitable photoinitiators include intermolecular hydrogen abstraction photoinitiators such as acryloyloxybenzophenone, 4-methacryloyloxyethoxybenzophenone, 4-methacryloyloxy-4'-methoxybenzophenone, 4-methacryloyloxyethoxy-4'-methoxybenzophenone, 4-methacryloyloxy-4'-bromobenzophenone, and 4-methacryloyloxyethoxy-4'-bromobenzophenone; and intramolecular hydrogen abstraction photoinitiators such as methylbenzoyl formate, methyl benzoylformate, oxyphenylacetic acid-2-(2-oxo-2-phenyl-acetoxy-ethoxy)ethyl ester, and oxyphenylacetic acid-2-(2-hydroxy-ethoxy)ethyl ester. These may be used alone or in combination of two or more.

[0120] Among the intermolecular hydrogen abstraction photoinitiators, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, and photoinitiators (c1) having a radically polymerizable functional group having a carbon-carbon double bond and a structure that generates radicals in the molecule, such as 4-acryloyloxybenzophenone, 4-methacryloyloxybenzophenone, 4-acryloyloxyethoxybenzophenone, 4-acryloyloxy-4'-methoxybenzophenone, 4-acryloyloxyethoxy-4'-methoxybenzophenone, and 4-methacryloyloxybenzophenone are preferred, and 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, 4-methacryloyloxybenzophenone, and 4-methacryloyloxybenzophenone are more preferred. The photoinitiator (c1) having a radical-polymerizable functional group having a carbon-carbon double bond and a structure that generates radicals in its molecule is incorporated into the polymerization structure after photoreaction, which tends to suppress bleed-out of the photoinitiator and improve the cohesive strength of the PSA sheet. Furthermore, intramolecular hydrogen abstraction photoinitiators are preferred because they can act not only as hydrogen donors in the system but also as starting points for radical generation, with methylbenzoyl formate being more preferred.

[0121] Examples of the cleavage-type photoinitiator include 2,2-dimethoxy-1,2-diphenylethan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)benzyl]phenyl}-2-methyl-propan-1-one, oligo(2-hydroxy-2-methyl-1-(4-(1-methylvinyl)phenyl)propanone), 2-benzyl-2-dimethylamino-1-(4-morpholino)-1-propanone, ... Examples of suitable amines include 2-(4-(4-morpholinophenyl)-2-butan-1-one, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, (2,4,6-trimethylbenzoyl)ethoxyphenylphosphine oxide, bis(2,6-dimethoxybenzoyl)2,4,4-trimethylpentylphosphine oxide, and derivatives thereof.

[0122] In the present invention, it is preferable that the photoinitiator (C) contains an intermolecular hydrogen abstraction photoinitiator and an intramolecular hydrogen abstraction photoinitiator, from the viewpoint of increasing the cohesive strength of the pressure-sensitive adhesive sheet.

[0123] Furthermore, in the present invention, the photoinitiator (C) preferably includes a photoinitiator (c1) having a radically polymerizable functional group with a carbon-carbon double bond and a structure that generates radicals in its molecule, and a hydrogen abstraction photoinitiator (c2) other than the photoinitiator (c1). The combined use of these photoinitiators (C) can enhance the cohesive strength of the pressure-sensitive adhesive sheets 1 and 2. Furthermore, when the pressure-sensitive adhesive sheets 1 and 2 are curable with active energy rays, they can be pressure-sensitive adhesive sheets that exhibit excellent secondary curing properties after being attached to an adherend. The hydrogen abstraction photoinitiator (c2) refers to a hydrogen abstraction photoinitiator other than the photoinitiator (c1) having a radically polymerizable functional group with a carbon-carbon double bond and a structure that generates radicals in its molecule. Among the hydrogen abstraction photoinitiators (c2), intramolecular hydrogen abstraction photoinitiators are preferred because they can act not only as hydrogen donors in the system but also as initiators of radical generation themselves, with methylbenzoyl formate being more preferred.

[0124] When the pressure-sensitive adhesive composition contains a photoinitiator (C), the content thereof is usually 10 parts by mass or less, preferably 5 parts by mass or less, more preferably 4 parts by mass or less, and particularly preferably 3 parts by mass or less, relative to 100 parts by mass of the acrylic polymer (A). The lower limit is usually 0.1 parts by mass. When two or more types of photoinitiators (C) are used in combination, the above content is the total amount of the photoinitiators (C) used.

[0125] When the photoinitiator (C) contains a photoinitiator (c1) having, in the molecule, a radical-polymerizable functional group having a carbon-carbon double bond and a structure that generates a radical, and a hydrogen abstraction photoinitiator (c2) other than the photoinitiator (c1), the mass ratio (c2 / c1) of the photoinitiator (c2) to the photoinitiator (c1) is preferably 0.5 to 10, more preferably 1 to 8, and even more preferably 2 to 6.

[0126] [Monofunctional (meth)acrylate] The pressure-sensitive adhesive composition may further contain a monofunctional (meth)acrylate having one (meth)acryloyl group, if necessary. By containing a monofunctional (meth)acrylate having one (meth)acryloyl group, the molecular weight between crosslinking points of the cured product can be increased, which is preferable in that the degree of freedom of movement of the molecular chain is increased and it becomes easier to obtain a cured product with excellent stress relaxation properties.

[0127] Examples of the monofunctional (meth)acrylate include ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, amyl (meth)acrylate, isoamyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, and dodecyl (meth)acrylate. (meth)acrylate, isododecyl (meth)acrylate, tetradecyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, behenyl (meth)acrylate, cyclopropyl (meth)acrylate, cyclobutyl (meth)acrylate, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, cycloheptyl (meth)acrylate, cyclooctyl (meth)acrylate, cyclononyl (meth)acrylate, cyclodecyl (meth)acrylate, isobornyl (meth)acrylate acrylate, norbornyl (meth)acrylate, adamantyl (meth)acrylate, tricyclodecane dimethanol acrylate, ethoxylated-o-phenylphenol acrylate, 2-hydroxy-o-phenylphenol propyl acrylate, methoxypolyethylene glycol (meth)acrylate, methoxypolypropylene glycol (meth)acrylate, polyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, phenoxyethylene glycol (meth)acrylate, phenoxydiethylene glycol benzyl (meth)acrylates such as chol (meth)acrylate, phenoxy polyethylene glycol (meth)acrylate, 2-hydroxy-o-phenylphenol propyl acrylate, 2-(meth)acryloyloxyethyl succinate, 2-(meth)acryloyloxyethyl tetrahydrophthalate, 2-(meth)acryloyloxyethyl hexahydrophthalate, 2-(meth)acryloyloxypropyl phthalate, 2-(meth)acryloyloxypropyl hydrophthalate, and 2-(meth)acryloyloxypropyl hexahydrophthalate;Benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxyethylene glycol (meth)acrylate, 2-naphthyl (meth)acrylate, 9-anthracenyl (meth)acrylate, 1-pyrenylmethyl (meth)acrylate, benzyl (meth)acrylate, tricyclodecane dimethanol monoacrylate monocarboxylic acid, dicyclopentanyl acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, trimethylolpropane mono(meth)acrylate, glycerin mono(meth)acrylate, pentaerythritol mono(meth)acrylate, diglycerin mono(meth)acrylate, ditrimethylolpropane mono(meth)acrylate, di Examples include pentaerythritol mono(meth)acrylate, ethoxylated trimethylolpropane mono(meth)acrylate, propoxylated trimethylolpropane mono(meth)acrylate, ethoxylated glycerin mono(meth)acrylate, propoxylated glycerin mono(meth)acrylate, ethoxylated pentaerythritol mono(meth)acrylate, propoxylated pentaerythritol mono(meth)acrylate, ethoxylated ditrimethylolpropane mono(meth)acrylate, propoxylated ditrimethylolpropane mono(meth)acrylate, alkylene oxide-modified diglycerin mono(meth)acrylate, and alkylene oxide-modified dipentaerythritol mono(meth)acrylate, as well as monofunctional oligomers such as monofunctional urethane (meth)acrylate, monofunctional epoxy (meth)acrylate, and monofunctional polyester (meth)acrylate. These may be used alone or in combination of two or more.

[0128] When the monofunctional (meth)acrylate component is contained, the content thereof is preferably 2 parts by mass or more, more preferably 4 parts by mass or more, and particularly preferably 6 parts by mass or more, relative to 100 parts by mass of the acrylic polymer (A), from the viewpoint of adjusting the crosslinking density and imparting appropriate flexibility to the cured product. The upper limit is preferably 20 parts by mass or less, more preferably 18 parts by mass or less, and particularly preferably 15 parts by mass or less.

[0129] [Other Components] The pressure-sensitive adhesive composition may contain, as needed, various additives such as silane coupling agents, ultraviolet absorbers, plasticizers, tackifiers, antioxidants, light stabilizers, metal deactivators, anti-aging agents, moisture absorbers, rust inhibitors, and inorganic particles as "other components" as long as the effects of the present invention are not impaired. Furthermore, the pressure-sensitive adhesive composition may contain, as needed, reaction catalysts such as tertiary amine compounds, quaternary ammonium compounds, and tin laurate compounds. These may be used alone or in combination of two or more. These may be used alone or in combination of two or more. It is particularly preferred that the pressure-sensitive adhesive composition contain a silane coupling agent.

[0130] [Silane coupling agent] The silane coupling agent is an organosilicon compound that contains one or more reactive functional groups and one or more alkoxy groups bonded to silicon atoms in its structure.The reactive functional groups include, for example, epoxy group, (meth)acryloyl group, mercapto group, hydroxyl group, carboxy group, amino group, amide group, and isocyanate group.Among these, epoxy group and mercapto group are preferred from the viewpoint of balance of durability.

[0131] The alkoxy group bonded to the silicon atom preferably contains an alkoxy group having 1 to 8 carbon atoms, from the viewpoint of durability and storage stability, and is particularly preferably a methoxy group or an ethoxy group. The silane coupling agent may also contain an organic substituent other than the reactive functional group and the alkoxy group bonded to the silicon atom, such as an alkyl group or a phenyl group.

[0132] Examples of the silane coupling agent include monomeric epoxy group-containing silane coupling agents, which are silane compounds such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; and silane coupling agents in which a part of the silane compound is hydrolyzed and condensed, or in which the silane compound is polymerized with methyltriethoxysilane, ethyltriethoxysilane, oligomeric epoxy group-containing silane coupling agents which are silane compounds obtained by co-condensation of alkyl group-containing silane compounds such as methyltrimethoxysilane and ethyltrimethoxysilane; monomeric mercapto group-containing silane coupling agents which are silane compounds such as 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, γ-mercaptopropyldimethoxymethylsilane and 3-mercaptopropylmethyldimethoxysilane; and silane coupling agents which are obtained by hydrolysis and condensation polymerization of a part of the silane compounds or by condensation polymerization of the silane compounds with methyl groups. oligomeric mercapto group-containing silane coupling agents which are silane compounds obtained by co-condensation of alkyl group-containing silane compounds such as 3-acryloxypropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane; (meth)acryloyl group-containing silane coupling agents such as 3-acryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane; coupling agents: amino group-containing silane coupling agents such as N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, and N-phenyl-3-aminopropyltrimethoxysilane; isocyanate group-containing silane coupling agents such as 3-isocyanatepropyltriethoxysilane;Examples of suitable silane coupling agents include vinyl group-containing silane coupling agents such as vinyltrimethoxysilane and vinyltriethoxysilane. These may be used alone or in combination of two or more.

[0133] Among these, epoxy group-containing silane coupling agents and mercapto group-containing silane coupling agents are preferably used because of their excellent durability, and among these, epoxy group-containing silane coupling agents are particularly preferred.

[0134] When the pressure-sensitive adhesive composition contains a silane coupling agent, the content thereof is usually 0.005 to 10 parts by mass, preferably 0.01 to 5 parts by mass, and particularly preferably 0.05 to 1 part by mass, relative to 100 parts by mass of the acrylic polymer (A). When the content is within the above range, adhesive strength and durability tend to be improved.

[0135] [Plasticizer] The plasticizer may be, but is not limited to, at least one selected from the group consisting of polyisobutylene, polyisoprene, polybutadiene, amorphous polyolefins and their copolymers, silicone, polyacrylate, oligomeric polyurethane, ethylene-propylene copolymer, etc., or any combination or mixture thereof. Among these, polyisobutylene is preferred. The polyisobutylene plasticizer may be, for example, one selected from the OPPANOLB series, which is commercially available from BASF under the trade name OPPANOL.

[0136] When the pressure-sensitive adhesive composition contains a plasticizer, the content thereof is not particularly limited and is usually 0.1 to 20 parts by mass, preferably 0.5 to 15 parts by mass, per 100 parts by mass of the acrylic polymer (A).

[0137] [Tackifier] The PSA composition may contain a tackifier to improve the adhesive strength of the PSA sheet. Examples of the tackifier include terpene resins such as polyterpenes (e.g., α-pinene resins, β-pinene resins, and limonene resins) and aromatic-modified polyterpene resins (e.g., phenol-modified polyterpene resins), coumaran-indene resins, petroleum-based resins such as C5 hydrocarbon resins, C9 hydrocarbon resins, C5 / C9 hydrocarbon resins, and dicyclopentadiene resins, and rosins such as modified rosin, hydrogenated rosin, polymerized rosin, and rosin esters.

[0138] When the pressure-sensitive adhesive composition contains a tackifier, the content thereof is not particularly limited and is usually 0.1 to 20 parts by mass, preferably 0.5 to 15 parts by mass, per 100 parts by mass of the acrylic polymer (A).

[0139] [Rust inhibitor] The pressure-sensitive adhesive composition may contain a rust inhibitor to prevent corrosion when the adherend includes a corrosive portion such as metal wiring, etc. Examples of the rust inhibitor include triazoles, benzotriazoles, etc.

[0140] When the pressure-sensitive adhesive composition contains a rust inhibitor, the content thereof is usually 0.01 to 5 parts by mass, preferably 0.1 to 3 parts by mass, per 100 parts by mass of the acrylic polymer (A).

[0141] <Method for manufacturing the present pressure-sensitive adhesive sheet 1> Next, a description will be given of a method for manufacturing the present pressure-sensitive adhesive sheet 1. However, the following description is an example of a method for manufacturing the present pressure-sensitive adhesive sheet 1, and the present pressure-sensitive adhesive sheet 1 is not limited to sheets manufactured by this manufacturing method.

[0142] The present pressure-sensitive adhesive sheet 1 can be produced by preparing a pressure-sensitive adhesive composition containing an acrylic polymer (A), preferably a crosslinking agent (B), a photoinitiator (C), and other components as necessary, forming the pressure-sensitive adhesive composition into a sheet, curing it by crosslinking, i.e., polymerization, and then processing it appropriately as necessary.

[0143] The pressure-sensitive adhesive composition may be prepared by kneading the raw materials using a temperature-controllable kneader (for example, a single-screw extruder, a twin-screw extruder, a planetary mixer, a twin-screw mixer, a pressure kneader, etc.). When kneading the various raw materials, various additives such as a silane coupling agent and an antioxidant may be blended together with a resin in advance and then fed to the kneader, or all materials may be melt-mixed in advance and then fed, or a masterbatch in which only the additives are concentrated in a resin may be prepared in advance and then fed.

[0144] The pressure-sensitive adhesive composition can be formed into a sheet by any known method, such as wet lamination, dry lamination, extrusion casting using a T-die, extrusion lamination, calendaring, inflation, injection molding, and liquid injection curing. Among these, when producing a sheet, wet lamination, extrusion casting, and extrusion lamination are preferred.

[0145] The pressure-sensitive adhesive composition can be cured by irradiating it with active energy rays, and the pressure-sensitive adhesive sheet 1 can be produced by irradiating a molded product of the pressure-sensitive adhesive composition, for example, a sheet, with active energy rays. In addition to irradiating it with active energy rays, the composition can also be further cured by heating.

[0146] Furthermore, the irradiation energy, irradiation time, irradiation method, etc. of the active energy rays are not particularly limited as long as they can activate the photoinitiator (C) and polymerize photoreactive components such as (meth)acrylic acid ester compounds. When a hydrogen abstraction photoinitiator is used as the photoinitiator (C), a hydrogen abstraction reaction also occurs from the acrylic polymer (A), and the acrylic polymer (A) is incorporated into the crosslinked structure, forming a crosslinked structure with many crosslinking points. Therefore, it is preferable that the pressure-sensitive adhesive sheet 1 be cured using a hydrogen abstraction photoinitiator.

[0147] Examples of the active energy rays in the active energy ray irradiation include light rays such as far ultraviolet rays, ultraviolet rays, near ultraviolet rays, infrared rays, and visible light rays, as well as ionizing radiation such as X-rays, α-rays, β-rays, γ-rays, electron beams, proton beams, and neutron beams. Among these, ultraviolet rays are preferred from the viewpoints of suppressing damage to optical device components and controlling reactions. Furthermore, ultraviolet rays are preferred from the viewpoints of curing speed, ease of availability of an irradiation device, cost, and the like.

[0148] Examples of light sources for ultraviolet irradiation include high-pressure mercury lamps, ultra-high-pressure mercury lamps, low-pressure mercury lamps, carbon arc lamps, metal halide lamps, xenon lamps, chemical lamps, electrodeless discharge lamps, and LED lamps, all of which emit light in the wavelength range of 150 to 450 nm. Of these, it is preferable to use high-pressure mercury lamps, metal halide lamps, and LED lamps.

[0149] The amount of active energy ray irradiation (cumulative light amount) is 100 to 10,000 mJ / cm from the viewpoint of curing. 2 is preferred, and more preferably 200 to 5000 mJ / cm 2 , and more preferably 300 to 4000 mJ / cm 2 , especially 400 to 3000 mJ / cm 2 , and even more so, 500 to 2000 mJ / cm 2 It is preferable to carry out the reaction under the following conditions.

[0150] It is preferable that the pressure-sensitive adhesive sheet 1 be pre-cured (primary cured) by irradiating it with active energy rays so that it has latent active energy ray curability, in other words, so that it retains active energy ray reactivity. When primary curing is performed by irradiating it with active energy rays, it is possible to adjust the degree of active energy ray crosslinking (gel fraction) by controlling the amount of active energy ray irradiation, but it is also possible to adjust the degree of active energy ray crosslinking (gel fraction) by using a filter or the like to partially block the active energy rays.

[0151] The present pressure-sensitive adhesive sheet 1 can also be provided as a pressure-sensitive adhesive sheet with a release film laminated on one or both sides thereof. In particular, from the viewpoint of preventing blocking and adhesion of foreign matter, it is preferable to coat both sides of the present pressure-sensitive adhesive sheet 1 with a release film.

[0152] When release films are provided on both sides of the present pressure-sensitive adhesive sheet 1, a laminate configuration in which a light release film with a relatively low release strength and a heavy release film with a relatively high release strength are laminated is preferred. When using a pressure-sensitive adhesive sheet with release films provided on both sides, first, one release film (light release film) is peeled off to expose one side of the pressure-sensitive adhesive sheet, which is then bonded to a component of an image display device (referred to as a first component), and the other release film (heavy release film) is peeled off to expose the other side of the pressure-sensitive adhesive sheet, which is then bonded to a component of an image display device (referred to as a second component).

[0153] As such a release film, a known release film can be appropriately used. As the base material for the release film, for example, a film such as a polyester film, a polyolefin film, a polycarbonate film, a polystyrene film, an acrylic film, a triacetyl cellulose film, or a fluororesin film that has been subjected to a release treatment by coating with a release agent such as a silicone resin, or release paper, etc., can be appropriately selected and used. Among these, a polyester film is preferred, a polyethylene terephthalate (PET) film is more preferred, and a biaxially oriented PET film is particularly preferred because of its excellent transparency, mechanical strength, heat resistance, flexibility, etc. Furthermore, a release film can be used in which a release layer formed by curing a curable silicone-based release agent containing a silicone resin as a main component is provided on the base material.

[0154] The thickness of the release film is not particularly limited, but from the viewpoint of processability and handling, the thickness is preferably 10 to 250 μm, more preferably 25 to 200 μm, and particularly preferably 35 to 190 μm.

[0155] In another embodiment of the method for producing the present pressure-sensitive adhesive sheet 1, the pressure-sensitive adhesive composition can be dissolved in an appropriate solvent and various coating methods can be used. When a coating method is used, the present pressure-sensitive adhesive sheet 1 can also be obtained by thermal curing in addition to the above-mentioned curing by irradiation with active energy rays. When a coating method is used, the thickness of the present pressure-sensitive adhesive sheet 1 can be adjusted by the coating thickness and the solids concentration of the coating liquid.

[0156] The coating method may be a conventional method such as roll coating, die coating, gravure coating, comma coating, screen printing, or bar coating.

[0157] To produce the present pressure-sensitive adhesive sheet 1 using the coating method, for example, the pressure-sensitive adhesive composition can be dissolved in a solvent, coated on the release film, dried, and cured by active energy ray irradiation to form the present pressure-sensitive adhesive sheet 1. Furthermore, a release film may be laminated on top as necessary. In this case, the pressure-sensitive adhesive composition may be coated on a release film, dried, cured by active energy ray irradiation, and then a release film may be laminated on top of that, or the pressure-sensitive adhesive sheet 1 may be formed by coating on a release film, drying, laminating a release film, and then curing by active energy ray irradiation.

[0158] The solvent is not particularly limited as long as it dissolves the pressure-sensitive adhesive composition, and examples thereof include ester solvents such as methyl acetate, ethyl acetate, butyl acetate, methyl acetoacetate, and ethyl acetoacetate; ketone solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; aromatic solvents such as toluene and xylene; and alcohol solvents such as methanol, ethanol, and propyl alcohol. These can be used alone or in combination of two or more. Among them, ethyl acetate, acetone, methyl ethyl ketone, and toluene are preferred in terms of solubility, drying properties, cost, and the like, and ethyl acetate is particularly preferred.

[0159] In view of drying properties, the content of the solvent is preferably 600 parts by mass or less, more preferably 500 parts by mass or less, even more preferably 400 parts by mass or less, and particularly preferably 300 parts by mass or less, relative to 100 parts by mass of the acrylic polymer (A), while being preferably 1 part by mass or more, more preferably 50 parts by mass or more, even more preferably 100 parts by mass or more, and particularly preferably 150 parts by mass or more.

[0160] The solvent content in the pressure-sensitive adhesive composition after drying is preferably 1% by mass or less, more preferably 0.5% by mass or less, particularly preferably 0.1% by mass or less, and most preferably 0% by mass.

[0161] The drying temperature is usually 40 to 150° C., more preferably 45 to 140° C., even more preferably 50 to 130° C., and particularly preferably 55 to 120° C. When the temperature is within this range, the solvent can be removed efficiently and relatively safely while suppressing thermal deformation of the release film.

[0162] The drying time is usually 1 to 30 minutes, more preferably 3 to 25 minutes, and even more preferably 5 to 20 minutes. When the drying time is within this range, the solvent can be removed efficiently and sufficiently.

[0163] Drying methods include, for example, drying with a dryer, drying with a heated roll, drying by blowing hot air onto the film, etc. Among these, using a dryer is preferred because it allows for uniform and easy drying. These methods can be used alone or in combination of two or more.

[0164] In yet another embodiment of the method for producing the present pressure-sensitive adhesive sheet 1, a pressure-sensitive adhesive composition may be prepared, coated onto a component of an image display device described below, and then cured to produce the present pressure-sensitive adhesive sheet 1. However, the method is not limited to this.

[0165] Furthermore, the present pressure-sensitive adhesive sheet 1 may be a single-layer pressure-sensitive adhesive sheet consisting of only an acrylic pressure-sensitive adhesive layer formed from a pressure-sensitive adhesive composition, or may be a multi-layer pressure-sensitive adhesive sheet in which other acrylic pressure-sensitive adhesive layers or other pressure-sensitive adhesive layers are laminated. In particular, the layer structure of the present pressure-sensitive adhesive sheet 1 is preferably at least two layers, more preferably at least three layers: an outermost layer, an innermost layer, and an intermediate layer, and particularly preferably at least three layers in which the outermost layer and the innermost layer are acrylic pressure-sensitive adhesive layers. Such a layer structure tends to result in a pressure-sensitive adhesive sheet that is less likely to be indented or dented even when localized pressure is applied.

[0166] When the pressure-sensitive adhesive sheet 1 has at least three layers, namely, a surface layer, a back layer, and an intermediate layer, the surface layer and the back layer (hereinafter also referred to as "surface and back layers") and the intermediate layer (the layer sandwiched between the surface layer and the back layer) are preferably formed from a pressure-sensitive adhesive composition containing acrylic polymers (A) of different compositions, particularly containing acrylic polymers (A) of different compositions as the main component. Such a layer configuration is advantageous in that contradictory physical properties such as stress relaxation and shape retention can be functionally separated for each layer. Furthermore, the surface layer and the back layer may be formed from a pressure-sensitive adhesive composition containing acrylic polymers (A) of different compositions, particularly containing acrylic polymers (A) of different compositions as the main component, but are preferably formed from a pressure-sensitive adhesive composition containing acrylic polymers (A) of the same composition.

[0167] When the pressure-sensitive adhesive sheet 1 has at least three layers (top layer / intermediate layer / rearmost layer) in which the top layer and the rearmost layer are acrylic pressure-sensitive adhesive layers, the top layer and the rearmost layer (surfaces to be attached to components of an image display device) are preferably high Tg layers. The intermediate layer sandwiched between the top layer and the rearmost layer is preferably a low Tg layer. Furthermore, the high Tg layers used in the top layer and the rearmost layer may have different glass transition temperatures (Tg), but the top layer and the rearmost layer preferably have the same glass transition temperature, and it is particularly preferred that the top layer and the rearmost layer be acrylic pressure-sensitive adhesive layers formed from the same pressure-sensitive adhesive composition.

[0168] The high Tg layer refers to a layer whose maximum value (glass transition temperature) of loss tangent (Tan δ) obtained by dynamic viscoelasticity measurement in the shear mode is usually −25° C. or higher, preferably −10° C. or higher, and particularly preferably 0° C. or higher. The upper limit of the glass transition temperature of the high Tg layer is usually 60° C. or lower, preferably 40° C. or lower, more preferably 30° C. or lower, and even more preferably 20° C. or lower. The low Tg layer refers to a layer whose maximum value (glass transition temperature) of loss tangent (Tan δ) obtained by dynamic viscoelasticity measurement in the shear mode is lower than the glass transition temperature of the high Tg layer, and whose glass transition temperature is usually 20° C. or lower, preferably 15° C. or lower, more preferably 10° C. or lower, even more preferably 8° C. or lower, particularly preferably 5° C. or lower, and most preferably 0° C. or lower. The lower limit of the glass transition temperature of the low Tg layer is usually −80° C., preferably −60° C. or higher, more preferably −50° C. or higher, and even more preferably −40° C. or higher.

[0169] Furthermore, when the pressure-sensitive adhesive sheet 1 has at least three layers, the outermost and innermost layers of which are acrylic pressure-sensitive adhesive layers, the ratio of the total thickness of the outermost and innermost layers to the total thickness is preferably 5 to 70%, more preferably 10 to 60%, and particularly preferably 20 to 45%. By setting the thicknesses of the outermost and innermost layers within the above ranges, a pressure-sensitive adhesive sheet can be obtained that is excellent in lamination suitability and durability, such as resistance to foaming at the peripheral edge, resistance to adhesive extrusion, and level difference absorbency.

[0170] The pressure-sensitive adhesive sheet 1 thus obtained is an optically transparent pressure-sensitive adhesive sheet. Here, "optically transparent" means that the total light transmittance is 80% or more, preferably 85% or more, and more preferably 90% or more. The haze value of the pressure-sensitive adhesive sheet is preferably 10% or less, more preferably 5% or less, and particularly preferably 3% or less.

[0171] The thickness of the present pressure-sensitive adhesive sheet 1 is preferably 50 to 1000 μm, more preferably 60 to 500 μm, and particularly preferably 75 to 300 μm.

[0172] Furthermore, the pressure-sensitive adhesive sheet 1 may be embossed or processed to have various irregularities (such as conical, pyramidal, or hemispherical shapes) as needed. Furthermore, in order to improve adhesion to various members, the surface may be subjected to various surface treatments such as corona treatment, plasma treatment, and primer treatment.

[0173] <Present Pressure-Sensitive Adhesive Sheet 2> As described above, the present pressure-sensitive adhesive sheet 2 has an acrylic pressure-sensitive adhesive layer, which is a cured reaction product formed from a syrup composition containing an alkyl(meth)acrylate (a1) and a hydroxyl group-containing monomer (a2) and / or a nitrogen-containing monomer (a3). Each component contained in the acrylic pressure-sensitive adhesive layer (syrup composition) will be described in detail below.

[0174] [Alkyl (meth)acrylate (a1)] Examples of the alkyl (meth)acrylate (a1) include the alkyl (meth)acrylate (a1) described in the present adhesive sheet 1, and the types of preferred monomers are also the same as those of the alkyl (meth)acrylate (a1) described in the present adhesive sheet 1.

[0175] The content of the structural units derived from the alkyl (meth)acrylate (a1) is preferably 5 to 95% by mass, more preferably 10 to 90% by mass, even more preferably 15 to 85% by mass, and particularly preferably 20 to 80% by mass, relative to the acrylic pressure-sensitive adhesive layer (syrup composition) in order to obtain flexibility. When the content of the structural units derived from the alkyl (meth)acrylate (a1) is equal to or greater than the lower limit, excellent resistance to foaming at the peripheral edge during lamination is obtained, and when the content is equal to or less than the upper limit, it is preferable in terms of achieving compatibility with other physical properties such as adhesiveness.

[0176] [Hydroxyl group-containing monomer (a2)] Examples of the hydroxyl group-containing (meta)monomer (a2) include the hydroxyl group-containing monomer (a2) described in the present adhesive sheet 1, and the types of preferred monomers are also the same as those of the hydroxyl group-containing (meta)monomer (a2) described in the present adhesive sheet 1.

[0177] When the acrylic pressure-sensitive adhesive layer (syrup composition) contains a structural unit derived from the hydroxyl group-containing monomer (a2), the content thereof is usually 3 to 30% by mass, preferably 5 to 25% by mass, and particularly preferably 7 to 20% by mass, relative to the acrylic pressure-sensitive adhesive layer (syrup composition). If the content is too low, the adhesive strength and moist heat resistance when used as a pressure-sensitive adhesive tend to decrease, whereas if the content is too high, the pressure-sensitive adhesive layer is more likely to undergo a self-crosslinking reaction, which tends to decrease heat resistance.

[0178] [Nitrogen-containing monomer (a3)] Examples of the nitrogen-containing monomer (a3) ​​include the nitrogen-containing monomer (a3) ​​described in the present adhesive sheet 1, and the types of preferred monomers are also the same as those of the nitrogen-containing monomer (a3) ​​described in the present adhesive sheet 1.

[0179] When the acrylic pressure-sensitive adhesive layer (syrup composition) contains a structural unit derived from the nitrogen-containing monomer (a3), the content thereof is usually 0.1 to 15 mass%, preferably 0.5 to 13 mass%, particularly preferably 1 to 10 mass%, and especially preferably 2 to 7 mass%, relative to the acrylic pressure-sensitive adhesive layer (syrup composition). If the content is too low, the adhesive strength and moist heat resistance when used as a pressure-sensitive adhesive tend to decrease, whereas if the content is too high, the pressure-sensitive adhesive layer is more likely to undergo a self-crosslinking reaction, which tends to decrease heat resistance.

[0180] The syrup composition may also contain the copolymerizable monomers (a4) to (a10) described above in connection with the present pressure-sensitive adhesive sheet 1. The types of these preferred monomers are the same as those described above in connection with the present pressure-sensitive adhesive sheet 1. The preferred content of the structural units derived from these copolymerizable monomers (a4) to (a10), i.e., the mass ratio relative to the acrylic pressure-sensitive adhesive layer (syrup composition), is the same as the mass ratio relative to all structural units of the acrylic polymer (A) described above in connection with the present pressure-sensitive adhesive sheet 1.

[0181] Furthermore, the acrylic adhesive layer preferably contains the crosslinking agent (B) and photoinitiator (C) described above in the present adhesive sheet 1, and may also contain other components such as a silane coupling agent described above in the present adhesive sheet 1.

[0182] [Crosslinking Agent (B)] When the crosslinking agent (B) is used, the preferred compounds and physical properties are the same as those of the crosslinking agent (B) described above for the present pressure-sensitive adhesive sheet 1. The preferred content of the crosslinking agent (B) is usually 0.1 to 20 mass%, preferably 0.5 to 15 mass%, and particularly preferably 1 to 10 mass%, relative to the acrylic pressure-sensitive adhesive layer (syrup composition). When the content is equal to or greater than the lower limit, poor curing tends to be prevented, while when the content is equal to or less than the upper limit, the film tends to have appropriate flexibility and excellent stress relaxation properties.

[0183] [Photoinitiator (C)] The photoinitiator is not particularly limited as long as it is the photoinitiator (C) described in the above-mentioned pressure-sensitive adhesive sheet 1, but from the viewpoint of efficiently progressing the polymerization reaction, it is preferable to contain a cleavage-type photoinitiator, and among the above-mentioned cleavage-type photoinitiators, 2,2-dimethoxy-1,2-diphenylethan-1-one, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and (2,4,6-trimethylbenzoyl)ethoxyphenylphosphine oxide are particularly preferred. Furthermore, from the viewpoint of efficiently forming a crosslinked structure, it is preferable to contain a hydrogen abstraction-type photoinitiator, and benzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, 4-phenylbenzophenone, 3,3'-dimethyl-4-methoxybenzophenone, and 4-(meth)acryloyloxybenzophenone are particularly preferred. The photoinitiator (C) may include one or more selected from the group consisting of cleavage-type photoinitiators and / or hydrogen abstraction-type photoinitiators.

[0184] When the photoinitiator (C) is used, its content is usually 0.1 to 10% by mass, preferably 0.5 to 6% by mass, and more preferably 1 to 4% by mass, relative to the acrylic pressure-sensitive adhesive layer (syrup composition). When the content is equal to or greater than the lower limit, poor curing tends to be prevented, while when the content is equal to or less than the upper limit, deterioration in stability such as precipitation from the pressure-sensitive adhesive sheet tends to be suppressed, and problems such as embrittlement and coloration tend to be suppressed.

[0185] [Monofunctional (meth)acrylate] When a monofunctional (meth)acrylate is used, the preferred compounds and physical properties are the same as those explained for the present pressure-sensitive adhesive sheet 1 above.

[0186] [Other Components] The other components may be the same as those described above for the present pressure-sensitive adhesive sheet 1. In particular, when a silane coupling agent is used, its content is usually 0.005 to 5 mass %, preferably 0.01 to 3 mass %, and more preferably 0.05 to 1 mass %, relative to the acrylic pressure-sensitive adhesive layer (syrup composition). When the content is within the above range, adhesive strength and durability tend to be improved.

[0187] The syrup component constituting the syrup composition in the present pressure-sensitive adhesive sheet 2 may be composed of an acrylic polymer (A) and a monomer component. In one example, such a syrup component may be formed by partial polymerization of the so-called monomer component, or may be prepared by adding the monomer component to a polymer in which the monomer components constituting the acrylic polymer (A) are completely or partially polymerized. That is, when a predetermined copolymerization component is partially polymerized, some of the monomers polymerize to form oligomers or polymers, while some of the monomers remain, thereby forming a syrup component. In another example, a syrup-like state can be obtained by adding the monomer component to a partially or completely polymerized polymer. Therefore, the term "monomer unit constituting the acrylic pressure-sensitive adhesive layer" as used herein may refer to a monomer present in the acrylic polymer component in the form of an oligomer or polymer, or a monomer contained in the syrup component before polymerization.

[0188] <Method for manufacturing the present pressure-sensitive adhesive sheet 2> Next, a description will be given of a method for manufacturing the present pressure-sensitive adhesive sheet 2. However, the following description is an example of a method for manufacturing the present pressure-sensitive adhesive sheet 2, and the present pressure-sensitive adhesive sheet 2 is not limited to sheets manufactured by this manufacturing method.

[0189] In producing the present pressure-sensitive adhesive sheet 2, a syrup composition is typically prepared by mixing an alkyl (meth)acrylate (a1) having an alkyl group containing 3 to 30 carbon atoms, a hydroxyl group-containing monomer (a2) and / or a nitrogen-containing monomer (a3), and optionally copolymerizable monomers (a4) to (a10), a photoinitiator (C), and the like. This syrup composition is then irradiated with active energy rays to allow prepolymerization. The syrup composition, to which additional photoinitiator (C), crosslinker (B), and other components are optionally added, is then coated onto a release film or the like using various coating methods, and the pressure-sensitive adhesive sheet 2 is then obtained by curing the syrup composition by irradiating with active energy rays or heating. The crosslinker and other components may be added to the syrup composition from the beginning, or may be added to the syrup composition after prepolymerization. Furthermore, prepolymerization and curing may be performed in a single step.

[0190] In another embodiment of the method for manufacturing the present adhesive sheet 2, the syrup composition is dissolved in a solvent, then coated on a release film and dried, and then prepolymerized and cured by irradiation with active energy rays, thereby forming the present adhesive sheet 2.

[0191] In the manufacturing method of the present pressure-sensitive adhesive sheet 2, the release film, active energy rays, solvent, etc., mixing method, coating method, drying conditions, etc. may be the same as those described in the manufacturing method of the present pressure-sensitive adhesive sheet 1 above.

[0192] The present pressure-sensitive adhesive sheet 2 obtained in this manner may be a single-layer sheet having only an acrylic pressure-sensitive adhesive layer, or a multi-layer sheet having multiple acrylic pressure-sensitive adhesive layers and other pressure-sensitive adhesive layers laminated thereon. The preferred layer configuration and thickness are the same as those of the present pressure-sensitive adhesive sheet 1. The present pressure-sensitive adhesive sheet 2 can also be provided as a pressure-sensitive adhesive sheet with a release film, which has a configuration in which a release film is laminated on one or both sides of an adhesive layer (the present pressure-sensitive adhesive sheet) made of a pressure-sensitive adhesive composition.

[0193] <Present Pressure-Sensitive Adhesive Sheet 3> A pressure-sensitive adhesive sheet according to one example of the third embodiment of the present invention (hereinafter referred to as "Present Pressure-Sensitive Adhesive Sheet 3") is a pressure-sensitive adhesive sheet formed from a pressure-sensitive adhesive composition containing an acrylic polymer (A), and has a glass transition temperature (Tg0) defined by the maximum value of Tan δ obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz, of -40 to 20°C, and a difference (ΔT) of 20°C or more between the temperature (T1) at or below the glass transition temperature (Tg0) at which the shear storage modulus (G') and the loss modulus (G") become equal, and the temperature (T2) at or above the glass transition temperature (Tg0) at which the shear storage modulus (G') and the loss modulus (G") become equal. The present pressure-sensitive adhesive sheet 3 will now be described.

[0194] The pressure-sensitive adhesive sheet 3 satisfies the following requirement (16): Requirement (16) The glass transition temperature (Tg0) defined as the maximum value of Tan δ obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz is −40 to 20° C.

[0195] A PSA sheet that satisfies requirement (16) has excellent handleability and resistance to adhesive extrusion. From this viewpoint, the glass transition temperature (Tg0) is preferably −30°C or higher, more preferably −25°C or higher, even more preferably −15°C or higher, particularly preferably −10°C or higher, and most preferably −5°C or higher. On the other hand, from the viewpoint of obtaining appropriate flexibility and stress relaxation, the upper limit is preferably 15°C or lower, more preferably 10°C or lower. The lower limit and upper limit of the glass transition temperature (Tg0) can be combined arbitrarily.

[0196] The pressure-sensitive adhesive sheet 3 further satisfies the following requirement (17): Requirement (17): The difference (ΔT) between the temperature (T1) at or below the glass transition temperature (Tg0) at which the shear storage modulus (G') and the loss modulus (G") become equal (hereinafter sometimes referred to as the "crossover point"), and the crossover point (T2) at or above the glass transition temperature (Tg0) (hereinafter sometimes referred to as the "crossover point interval") is 20°C or greater.

[0197] A PSA sheet that satisfies requirement (17) can be laminated without air bubbles up to the peripheral edge near the edge of the PSA sheet. The temperature range from the crossover point (T1) to the crossover point (T2) is a region in which the loss modulus (G") exceeds the shear storage modulus (G'). The fact that the loss modulus (G") exceeds the shear storage modulus (G') indicates that, of the energy generated by strain due to foaming, the energy component released to the outside is greater than the energy component accumulated inside the PSA sheet, and air bubbles are likely to disappear. In other words, the crossover point interval (ΔT) is the size of the temperature region in which air bubbles are likely to disappear, and if this range is 20°C or higher, air taken in during lamination of components is likely to diffuse, resulting in the reduction or elimination of air bubbles at the peripheral edge of the PSA sheet.

[0198] In laminates requiring precision lamination, such as laminates for image display devices, finishing lamination is typically performed by heating and pressurizing using an autoclave when laminating components. After the autoclave process is completed or after the product begins to be used, air bubbles may form at the peripheral edges. One of the main causes of these bubbles is thought to be the infiltration of air present in the autoclave oven between the laminating components and the pressure-sensitive adhesive sheet due to the high pressure inside the oven during the lamination process. Conventionally, these air bubbles were not visible because the peripheral edges of displays were covered by a concealing layer such as a printed layer or a bezel. However, in recent years, due to demands for narrower display frames and frameless designs, the peripheral edges have become narrower, and there is a strong demand for improved bubble resistance at the peripheral edges of pressure-sensitive adhesive sheets.

[0199] From the viewpoint of improving the foaming resistance at the peripheral edge of the PSA sheet, the crossover point interval (ΔT) is preferably 22° C. or more, more preferably 25° C. or more, even more preferably 28° C. or more, and particularly preferably 30° C. or more. On the other hand, from the viewpoint of shape stability, the upper limit of the crossover point is preferably 100° C. or less, more preferably 80° C. or less, even more preferably 60° C. or less, particularly preferably 50° C. or less, and especially preferably 40° C. or less. The lower limit and upper limit of the crossover point interval (ΔT) can be combined in any manner.

[0200] The glass transition temperature (Tg0) and crossover point interval (ΔT) are measured, for example, as follows. Pressure-sensitive adhesive sheets are repeatedly laminated to a thickness of 0.7 to 1.2 mm (e.g., 0.8 mm), and then punched out into a circular shape with a diameter of 8 mm to obtain a sample. The obtained sample is subjected to dynamic viscoelasticity measurement using a rheometer under the following conditions: measurement jig: 8 mm diameter parallel plates, frequency: 1 Hz, measurement temperature: -50 to 150°C, and heating rate: 5°C / min. From the obtained dynamic viscoelasticity spectrum, the temperature at which Tan δ reaches its maximum value (glass transition temperature (Tg0)) is determined. Then, the temperature (crossover point) (T1) at which the shear storage modulus (G') and the loss modulus (G") become equal in the temperature range lower than the glass transition temperature (Tg0), and the crossover point (T2) at or above the glass transition temperature are read, and the crossover point interval (ΔT) is calculated using the following formula: Crossover point interval (ΔT) = (T2) - (T1) Note that "adjusted to a thickness of 0.7 to 1.2 mm" means that if the thickness of the PSA sheet used as the measurement sample does not fall within this range, the thickness of the measurement sample is adjusted to fall within this range by, for example, stacking several sheets. The same applies when the thickness of the measurement sample is specified in other tests.

[0201] The loss tangent (Tan δ) is preferably 1.2 or more, more preferably 1.3 or more, and particularly preferably 1.5 or more, while the upper limit is preferably 5 or less, more preferably 4.5 or less, and particularly preferably 4 or less.

[0202] Examples of methods for adjusting the glass transition temperature (Tg0) and the crossover point interval (ΔT) within the above ranges include, but are not limited to, a method of adjusting the composition or molecular weight of the acrylic polymer (A) described below, or the type or content of the crosslinking agent (B) or the photoinitiator (C), as well as a method of adjusting the amount of active energy ray irradiation.

[0203] It is preferable that the pressure-sensitive adhesive sheet 3 further satisfies the following requirement (18): Requirement (18) The shear storage modulus (G0'(25°C)) at 25°C, obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz, is 50 kPa or more.

[0204] PSA sheets that satisfy requirement (18) tend to have excellent handleability and resistance to adhesive extrusion. From this viewpoint, the shear storage modulus at 25°C (G0'(25°C)) is preferably 60 kPa or more, more preferably 70 kPa or more, and particularly preferably 80 kPa or more. On the other hand, from the viewpoint of ensuring the stress relaxation properties of the PSA sheet, the shear storage modulus at 25°C (G0'(25°C)) is preferably 1000 kPa or less, more preferably 900 kPa or less, even more preferably 800 kPa or less, and particularly preferably 500 kPa or less. The lower limit and upper limit of the shear storage modulus at 25°C (G0'(25°C)) can be combined in any manner.

[0205] It is preferable that the pressure-sensitive adhesive sheet 3 further satisfies the following requirement (19): Requirement (19) The shear storage modulus at 85°C (G0'(85°C)) obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz is 100 kPa or less.

[0206] PSA sheets that satisfy requirement (19) tend to have excellent handleability and resistance to adhesive extrusion. From this viewpoint, the shear storage modulus at 85°C (G0'(85°C)) is preferably 80 kPa or less, more preferably 50 kPa or less, and particularly preferably 30 kPa or less. On the other hand, from the viewpoint of ensuring the stress relaxation properties of the PSA sheet, the shear storage modulus at 85°C (G0'(85°C)) is preferably 5 kPa or more, more preferably 7 kPa or more, and even more preferably 10 kPa or more. The lower limit and upper limit of the shear storage modulus at 85°C (G0'(85°C)) can be combined in any manner.

[0207] The shear storage modulus at 25°C (G'(25°C)) and the shear storage modulus at 85°C (G'(85°C)) can be obtained by reading the value of the shear storage modulus at 25°C (G'(25°C)) and the value of the shear storage modulus at 85°C (G'(85°C)) from dynamic viscoelasticity spectrum data in shear mode obtained in the same manner as in the measurement of the glass transition temperature (Tg) and the crossover point interval (ΔT) described above.

[0208] Examples of methods for adjusting the shear storage modulus at 25°C (G'(25°C)) and the shear storage modulus at 85°C (G'(85°C)) within the above ranges include a method of adjusting the composition or molecular weight of the acrylic polymer (A) or the type or content of the crosslinking agent (B) or the photoinitiator (C), as well as a method of adjusting the amount of active energy ray irradiation. However, the methods are not limited to these.

[0209] Furthermore, from the same viewpoint as in the case of the pressure-sensitive adhesive sheets 1 and 2, it is preferable that the pressure-sensitive adhesive sheet 3 satisfies the above-mentioned requirements (6) and (7).

[0210] The pressure-sensitive adhesive sheet 3 is preferably active energy ray-curable. Here, the term "active energy ray-curable" means that the pressure-sensitive adhesive sheet has the property of being curable by active energy rays, in other words, that there is room for curing by active energy rays.

[0211] The present pressure-sensitive adhesive sheet 3 may be cured to a state where there is still room for curing by active energy rays (hereinafter also referred to as "primary curing"), or it may be uncured (hereinafter also referred to as "uncured") and be curable by active energy rays. A primarily cured or uncured pressure-sensitive adhesive sheet can be cured (hereinafter also referred to as "secondary curing") by irradiating it with active energy rays after being attached to an adherend. When the present pressure-sensitive adhesive sheet 3 is active energy ray-curable, it preferably satisfies the following requirements.

[0212] Requirement (20) The adhesive sheet is exposed to active energy rays with a wavelength of 365 nm with an integrated light intensity of 2000 to 4000 mJ / cm 2 When irradiated so as to satisfy the above condition, the shear storage modulus (G1'(25°C)) at 25°C after curing is 60 kPa or more, as determined by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz.

[0213] A pressure-sensitive adhesive sheet satisfying requirement (20) tends to exhibit high cohesive strength after exposure to active energy rays. From the viewpoint of obtaining high cohesive strength, the shear storage modulus at 25°C after curing (G1'(25°C)) is preferably 70 kPa or more, more preferably 100 kPa or more, and even more preferably 120 kPa or more. On the other hand, from the viewpoint of obtaining stress relaxation properties, the shear storage modulus at 25°C after curing (G1'(25°C)) is preferably 1000 kPa or less, more preferably 400 kPa or less, and even more preferably 200 kPa or less. The lower and upper limits of the shear storage modulus at 25°C after curing (G1'(25°C)) can be arbitrarily combined. The method for measuring the shear storage modulus at 25°C after curing (G1'(25°C)) is the same as that for the shear storage modulus at 25°C (G0'(25°C)).

[0214] Requirement (21) The adhesive sheet is exposed to active energy rays having a wavelength of 365 nm with an integrated light intensity of 2000 to 4000 mJ / cm 2 When irradiated so as to satisfy the above condition, the shear storage modulus (G1'(85°C)) at 85°C after curing, as determined by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz, is 10 kPa or more.

[0215] A pressure-sensitive adhesive sheet satisfying requirement (21) tends to have high cohesive strength after exposure to active energy rays. From the viewpoint of obtaining high cohesive strength, the shear storage modulus at 85°C after curing (G1'(85°C)) is preferably 20 kPa or more, more preferably 30 kPa or more, and even more preferably 40 kPa or more. On the other hand, from the viewpoint of obtaining stress relaxation properties, the shear storage modulus at 85°C after curing (G1'(85°C)) is preferably 300 kPa or less, more preferably 200 kPa or less, and even more preferably 100 kPa or less. The lower and upper limits of the shear storage modulus at 85°C after curing (G1'(85°C)) can be arbitrarily combined. The method for measuring the shear storage modulus at 85°C after curing (G1'(85°C)) is the same as that for the shear storage modulus at 25°C (G0'(85°C)).

[0216] Requirement (22) The adhesive sheet is exposed to active energy rays with a wavelength of 365 nm with an integrated light intensity of 2000 to 4000 mJ / cm 2 When the composition is irradiated so as to satisfy the above condition, the glass transition temperature (Tg1) after curing, which is defined as the maximum value of Tan δ obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz, is −40° C. or higher.

[0217] A pressure-sensitive adhesive sheet that satisfies requirement (22) tends to have high cohesive strength after exposure to active energy rays. From the viewpoint of obtaining high cohesive strength, the glass transition temperature (Tg1) after curing is preferably −35° C. or higher, more preferably −30° C. or higher, and even more preferably −25° C. or higher. On the other hand, from the viewpoint of obtaining stress relaxation properties, the glass transition temperature (Tg1) after curing is preferably 20° C. or lower, more preferably 10° C. or lower, and even more preferably 0° C. or lower. The lower limit and upper limit of the glass transition temperature (Tg) can be arbitrarily combined. The method for measuring the glass transition temperature (Tg1) after curing is the same as that for the glass transition temperature (Tg0).

[0218] Furthermore, from the same viewpoint as in the case of the pressure-sensitive adhesive sheets 1 and 2, it is preferable that the pressure-sensitive adhesive sheet 3 satisfies the above-mentioned requirements (14) and (15).

[0219] The present pressure-sensitive adhesive sheet 3 has an acrylic pressure-sensitive adhesive layer formed from a pressure-sensitive adhesive composition containing an acrylic polymer (A). The acrylic resin (A) is preferably the main component of the pressure-sensitive adhesive composition. The pressure-sensitive adhesive composition preferably contains a crosslinking agent (B). The pressure-sensitive adhesive composition preferably contains a photoinitiator (C). The pressure-sensitive adhesive composition may further contain components other than the acrylic polymer (A), the crosslinking agent (B), and the photoinitiator (C). When the pressure-sensitive adhesive composition is active energy ray-curable, the present pressure-sensitive adhesive sheet 3 is typically obtained by curing a pressure-sensitive adhesive composition containing the acrylic polymer (A) and the photoinitiator (C). Examples of the acrylic polymer (A) used in the present pressure-sensitive adhesive sheet 3 include the acrylic polymer (A) described above for the present pressure-sensitive adhesive sheet 1. The preferred content of the copolymerization component of the acrylic polymer (A), i.e., the preferred mass ratio of each structural unit relative to the acrylic polymer (A), is also the same as that described for the present pressure-sensitive adhesive sheet 1. When a crosslinking agent (B) and / or a photoinitiator (C) is used, the preferred compounds and their contents are the same as those described for the present pressure-sensitive adhesive sheet 1. Furthermore, the present pressure-sensitive adhesive sheet 3 may contain other components such as a silane coupling agent, as described for the present pressure-sensitive adhesive sheet 1, and the preferred compounds and their contents are the same as those described for the present pressure-sensitive adhesive sheet 1.

[0220] <Method for manufacturing the present adhesive sheet 3> Next, a description will be given of a method for manufacturing the present adhesive sheet 3. However, the following description is an example of a method for manufacturing the present adhesive sheet 3, and the present adhesive sheet 3 is not limited to sheets manufactured by this manufacturing method.

[0221] The present pressure-sensitive adhesive sheet 3 can be produced by preparing a pressure-sensitive adhesive composition containing an acrylic polymer (A), preferably a crosslinking agent (B), a photoinitiator (C), and other components as necessary, molding the pressure-sensitive adhesive composition into a sheet, curing it by crosslinking, i.e., polymerization, and then processing it appropriately as necessary. In the method for producing the present pressure-sensitive adhesive sheet 3, the release film, active energy rays, solvent, etc., as well as the mixing method, coating method, drying conditions, etc., may be the same as those described above for the present pressure-sensitive adhesive sheet 1.

[0222] The present pressure-sensitive adhesive sheet 3 obtained in this manner may be a single-layer sheet having only an acrylic pressure-sensitive adhesive layer, or a multi-layer sheet having multiple acrylic pressure-sensitive adhesive layers and other pressure-sensitive adhesive layers laminated thereon. The preferred layer configuration and thickness are the same as those of the present pressure-sensitive adhesive sheet 1. The present pressure-sensitive adhesive sheet 3 can also be provided as a pressure-sensitive adhesive sheet with a release film, which has a configuration in which a release film is laminated on one or both sides of an adhesive layer (the present pressure-sensitive adhesive sheet) made of a pressure-sensitive adhesive composition.

[0223] <Preferred uses of the present pressure-sensitive adhesive sheet> The present pressure-sensitive adhesive sheets 1 and 2 and the present pressure-sensitive adhesive sheet 3 (hereinafter sometimes collectively referred to as "the present pressure-sensitive adhesive sheet") are suitable for use in bonding optical components. Specifically, they are suitable for use in bonding components constituting a display, particularly components used in producing a display, and are suitable for use as pressure-sensitive adhesive sheets for bonding image display device components such as an image display panel and a protective panel or touch panel arranged on the front side (viewing side) of the image display device, or components constituting the image display device components. Note that the same image display device components as those described below can be used.

[0224] <<Laminate for Image Display Device>> A laminate for an image display device according to one example of the embodiment of the present invention (hereinafter, may be referred to as "the present laminate for an image display device") is a laminate for an image display device having a configuration in which two components of the image display device are laminated with the present pressure-sensitive adhesive sheet interposed therebetween. The present laminate for an image display device is preferably a laminate for an image display device having a configuration in which two components of the image display device are laminated with the present pressure-sensitive adhesive sheet interposed therebetween.

[0225] Of the components of the laminate for an image display device, the pressure-sensitive adhesive sheet has been described above, and the components other than the pressure-sensitive adhesive sheet will be described below.

[0226] <Image Display Device Components> Examples of image display device components constituting the present laminate for an image display device include flat panel image display device components, curved image display device components, and flexible image display device components. Examples of such image display device components include image display panels such as liquid crystal displays and organic electroluminescence (EL) displays, surface protection panels (surface protection films), polarizing plates, polarizing elements, retardation films, color filters, barrier films, viewing angle compensation films, brightness enhancement films, contrast enhancement films, diffusion films, semi-transmitting reflective films, electrode films, transparent conductive films, metal mesh films, and touch sensor films. Any one of these may be used alone or in combination. Examples include a combination of a surface protection panel with another image display device component, or a combination with another image display device component.

[0227] Preferably, one of the two image display device components is a surface protection panel, and the other is a component consisting of one or a combination of two or more components selected from the group consisting of a touch sensor film, an image display panel, a color filter, a polarizing element, and a retardation film. It is more preferable that the surface protection panel has a frame-shaped concealing portion on its periphery, with the frame having a portion with a width of 3 mm or less. With this configuration, the effects of the present invention can be particularly achieved. From this perspective, a panel having a portion with a frame width of 2 mm or less is particularly preferable, and a panel having a portion with a width of 1.5 mm or less is particularly preferable.

[0228] The present laminate for an image display device is preferably fixed in a curved shape. Since the present pressure-sensitive adhesive sheet also has excellent reliability in laminating to curved parts, the above-mentioned configuration allows the effects of the present invention to be particularly enjoyed.

[0229] <Method for manufacturing the present laminate for an image display device> The method for manufacturing the present laminate for an image display device is not particularly limited, and as described above, for example, the pressure-sensitive adhesive composition may be applied to a component of an image display device to form a pressure-sensitive adhesive sheet, or a pressure-sensitive adhesive sheet with a release film may be formed in advance and then laminated to a component of an image display device.

[0230] <<Image Display Device>> An image display device according to an embodiment of the present invention (hereinafter, sometimes referred to as the "image display device") incorporates a laminate for an image display device, which has a configuration in which two image display device components are bonded together via the present pressure-sensitive adhesive sheet. For example, an image display device may have a structure in which a laminate for an image display device, which has a configuration in which two image display device components are bonded together via the present pressure-sensitive adhesive sheet, is combined with other image display device components. In this case, "other image display device components" may include, for example, FPC cables, reflective sheets, light guide plates and light sources, diffusion films, prism sheets, liquid crystal panels, organic EL panels, anti-reflection films, color filters, polarizing plates, retardation plates, glass substrates, surface protection films, and integrated composites of these components. Specific examples of the image display device include liquid crystal displays, organic EL displays, inorganic EL displays, electronic paper, plasma displays, and microelectromechanical system (MEMS) displays used in personal computers, mobile devices, game consoles, televisions (TVs), car navigation systems, touch panels, pen tablets, etc.

[0231] The present invention will be explained in more detail below by way of examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the invention.

[0232] Prior to the examples, the following raw materials were prepared.

[0233] [Acrylic Polymer (A)] Acrylic polymers (A-1) to (A-4) having copolymer component compositions and weight average molecular weights (Mw) as shown in Table 1 below were prepared.

[0234]

[0235] [Crosslinking agent (B)] (B-1): Polypropylene glycol #400 diacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd., "NK Ester APG-400") (B-2): Propoxylated pentaerythritol tri- and tetraacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd., "NK Ester ATM-4PL") (B-3): Pentaerythritol tri- and tetraacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd., "NK Ester ATMM-3L")

[0236] [Photoinitiator (C)] (C-1): Methylbenzoyl formate ("Omnirad MBF" manufactured by IGM) (C-2): 4-methallyloyloxybenzophenone ("MBP" manufactured by Shinryo Corporation) (C-3): Mixture of 2,4,6-trimethylbenzophenone and 4-methylbenzophenone ("Esacure TZT" manufactured by IGM)

[0237] [Others] Silane coupling agent: 3-glycidyloxypropyltrimethoxysilane ("KBM403" manufactured by Shin-Etsu Chemical Co., Ltd.)

[0238] Example 1-1 100 parts by mass of an acrylic polymer (A-1), 1.5 parts by mass of a crosslinking agent (B-1), 2.45 parts by mass of a photoinitiator (C-1), 1.05 parts by mass of a photoinitiator (C-2), and 0.2 parts by mass of a silane coupling agent were uniformly mixed to prepare a pressure-sensitive adhesive composition.

[0239] Next, the pressure-sensitive adhesive composition was spread in a sheet form on a 100 μm-thick release film (a PET film manufactured by Mitsubishi Chemical Corporation) that had been subjected to a silicone release treatment so that the thickness of the pressure-sensitive adhesive composition was 150 μm. In addition, a 75 μm-thick release film (a PET film manufactured by Mitsubishi Chemical Corporation) that had been subjected to a silicone release treatment was laminated on the sheet-like pressure-sensitive adhesive composition. Thereafter, a high-pressure mercury lamp was used to irradiate the pressure-sensitive adhesive composition with an integrated light intensity of 440 mJ / cm at a wavelength of 365 nm. 2 Both surfaces of the sheet-like pressure-sensitive adhesive composition were irradiated with active energy rays via the release film so as to obtain a pressure-sensitive adhesive sheet with a release film consisting of release film / pressure-sensitive adhesive sheet / release film. The pressure-sensitive adhesive sheet of Example 1-1 was a pressure-sensitive adhesive sheet equipped with active energy ray curability, which was cured by irradiation with active energy rays.

[0240] Examples 1-2 to 1-5 PSA sheets with release films were prepared in the same manner as in Example 1-1, except that the formulation, thickness, and integrated light amount were changed as shown in Table 2. The PSA sheets of Examples 1-2 to 1-5 were PSA sheets with active energy ray curability, which means that they were cured by irradiation with active energy rays.

[0241] Example 1-6 100 parts by mass of an acrylic polymer (A-1), 1.5 parts by mass of a crosslinking agent (B-1), 2.45 parts by mass of a photoinitiator (C-1), 1.05 parts by mass of a photoinitiator (C-2), and 0.2 parts by mass of a silane coupling agent were prepared and uniformly mixed to form a pressure-sensitive adhesive composition for the front and back layers. On the other hand, 100 parts by mass of an acrylic polymer (A-4), 15 parts by mass of a crosslinking agent (B-3), and 2.0 parts by mass of a photoinitiator (C-3) were prepared and uniformly mixed to form a pressure-sensitive adhesive composition for the intermediate layer. The pressure-sensitive adhesive composition for the front and back layers and the pressure-sensitive adhesive composition for the intermediate layer were each fed into two extruders and co-extruded in a two-kind, three-layer structure (outermost layer / intermediate layer / outermost layer, thickness ratio 1:2:1), followed by hot-melt molding into a 150 μm-thick sheet.

[0242] Next, the sheet-like pressure-sensitive adhesive composition was sandwiched between two polyethylene terephthalate films (a PET film manufactured by Mitsubishi Chemical Corporation, thickness 100 μm, and a PET film manufactured by Mitsubishi Chemical Corporation, thickness 75 μm) whose surfaces had been treated with silicone release agent, i.e., two release films, to obtain a laminate consisting of release film / pressure-sensitive adhesive composition / release film. Thereafter, a high-pressure mercury lamp was used to irradiate the laminate with an integrated light intensity of 500 mJ / cm at a wavelength of 365 nm. 2 Both surfaces of the sheet-form pressure-sensitive adhesive composition were irradiated with active energy rays via the release film so as to obtain a pressure-sensitive adhesive sheet with a release film consisting of release film / pressure-sensitive adhesive sheet / release film. The pressure-sensitive adhesive sheet of Example 1-6 was a pressure-sensitive adhesive sheet equipped with active energy ray curability, which was cured by irradiation with active energy rays.

[0243] Example 1-7 A pressure-sensitive adhesive sheet with a release film was produced in the same manner as in Example 1-6, except that the formulation, thickness, layer composition ratio, and integrated light amount were changed to those shown in Table 2. The pressure-sensitive adhesive sheet of Example 1-7 was an active energy ray-curable pressure-sensitive adhesive sheet that was cured by irradiation with active energy rays.

[0244] Comparative Example 1-1 A pressure-sensitive adhesive sheet with a release film was produced in the same manner as in Example 1-1, except that the formulation, thickness, and integrated light amount were changed to those shown in Table 2. The pressure-sensitive adhesive sheet of Comparative Example 1-1 was an active energy ray-curable pressure-sensitive adhesive sheet that was cured by irradiation with active energy rays.

[0245] Comparative Example 1-2 A pressure-sensitive adhesive sheet with a release film was produced in the same manner as in Example 1-6, except that the formulation, thickness, layer composition ratio, and integrated light amount were changed to those shown in Table 2. The pressure-sensitive adhesive sheet of Comparative Example 1-2 was an active energy ray-curable pressure-sensitive adhesive sheet that was cured by irradiation with active energy rays.

[0246]

[0247] [Measurement and Evaluation of Physical Properties] The pressure-sensitive adhesive sheets produced in Examples 1-1 to 1-7 and Comparative Examples 1-1 and 1-2 were subjected to the following various measurements and evaluations. The evaluation results are summarized in Table 3 below.

[0248] [Shear storage modulus at 25°C (G0'(25°C))] The release film on one side was removed from the pressure-sensitive adhesive sheets with release films prepared in the Examples and Comparative Examples, and the sheets were repeatedly laminated with a hand roller to a thickness of approximately 0.8 mm, and then punched out into circles with a diameter of 8 mm to prepare samples. The obtained samples were placed in a rheometer ("DHR-2" manufactured by T.A. Instruments) and subjected to dynamic viscoelasticity measurement under the conditions of measurement jig: 8 mm diameter parallel plates, frequency: 1 Hz, measurement temperature: -50 to 150°C, and heating rate: 5°C / min, and the value of shear storage modulus at 25°C (G0'(25°C)) was read.

[0249] Furthermore, the pressure-sensitive adhesive sheets with release films prepared in the Examples and Comparative Examples were cured by irradiating the pressure-sensitive adhesive sheets with light through the release film using a metal halide lamp so that the active energy rays having a wavelength of 365 nm achieved the integrated light amount shown in Table 3 below. Using the cured pressure-sensitive adhesive sheets, the shear storage modulus at 25°C after curing (G1'(25°C)) was measured in the same manner as the shear storage modulus before light irradiation (G0'(25°C)).

[0250] [Glass Transition Temperature] The release film on one side of the pressure-sensitive adhesive sheets with release film prepared in the Examples and Comparative Examples was removed, and the sheets were repeatedly laminated with a hand roller to a thickness of approximately 0.8 mm. Then, a circle with a diameter of 8 mm was punched out to prepare a sample. The obtained sample was placed in a rheometer ("DHR-2" manufactured by T.A. Instruments) and subjected to dynamic viscoelasticity measurement under the following conditions: measurement jig: 8 mm diameter parallel plates; frequency: 1 Hz; measurement temperature: -50 to 150 °C; heating rate: 5 °C / min. The glass transition temperature (Tg0), defined as the maximum value of Tan δ obtained by dynamic viscoelasticity measurement in shear mode at a frequency of 1 Hz, was determined. Note that in Examples 1-5, two maximum values ​​were observed in the dynamic viscoelasticity measurement, and the temperature showing the larger maximum value was recorded in the table as the glass transition temperature (Tg0).

[0251] Furthermore, the pressure-sensitive adhesive sheets with release films produced in the Examples and Comparative Examples were cured by irradiating the pressure-sensitive adhesive sheets with active energy rays having a wavelength of 365 nm through the release film using a metal halide lamp so that the integrated light intensity was as shown in Table 3 below. Using the cured pressure-sensitive adhesive sheets, the glass transition temperature (Tg1) after curing was determined in the same manner as the glass transition temperature before light irradiation.

[0252] [Stress Relaxation Rate] The release film on one side was removed from the pressure-sensitive adhesive sheets with release film prepared in the Examples and Comparative Examples, and the sheets were repeatedly laminated with a hand roller to a thickness of approximately 0.8 mm. A circle with a diameter of 25 mm was punched out to prepare a sample. A viscoelasticity measuring device (T.A. Instruments "DHR2") was used to apply a 25% strain to the obtained sample at 70 ° C., and the storage modulus after 0.1 seconds was read as the initial modulus (G '(0)). Furthermore, a 25% strain was applied at a temperature of 70 ° C., and the storage modulus after 300 seconds was read as the relaxation modulus (G '(300)). The values ​​of the initial modulus (G '(0)) and the relaxation modulus (G '(300)) were substituted into the following formula (I) to determine the stress relaxation rate (X ). Stress relaxation rate (X0)=(G0'(300) / G0'(0)) (I)

[0253] Furthermore, the pressure-sensitive adhesive sheets with release films produced in the Examples and Comparative Examples were irradiated with light through the release film using a metal halide lamp, with active energy rays having a wavelength of 365 nm, so that the integrated light intensity was as shown in Table 3 below, thereby curing the pressure-sensitive adhesive sheets. Using the cured pressure-sensitive adhesive sheets, the initial elastic modulus (G1'(0)) and relaxation elastic modulus (G1'(300)) after curing were measured in the same manner as in the measurement of the stress relaxation modulus before light irradiation. The initial elastic modulus (G1'(0)) and relaxation elastic modulus (G1'(300)) after curing were substituted into the following formula (II) to determine the stress relaxation modulus after curing (X1). Stress relaxation modulus after curing (X1) = (G1'(300) / G1'(0)) (II)

[0254] Further, the difference (X1-X0) between the stress relaxation rate before and after curing was calculated from the stress relaxation rate (X0) and the stress relaxation rate after curing (X1).

[0255] [Gel Fraction] For the pressure-sensitive adhesive sheets with release films prepared in the Examples and Comparative Examples, approximately 0.1 g of pressure-sensitive adhesive sheet pieces were collected from the pressure-sensitive adhesive sheets after peeling off the release films. The collected pressure-sensitive adhesive sheet pieces were wrapped in a bag-shaped SUS mesh (#150) with a mass (X), and the bag was closed to prepare a sample, and the mass (Y) of the sample was measured. The sample was immersed in ethyl acetate and stored in a dark place at 23°C for 24 hours, and then removed and heated at 70°C for 4.5 hours to evaporate the ethyl acetate, and the mass (Z) of the dried sample was measured. The gel fraction before light irradiation was calculated from each measured mass using the following formula: Gel Fraction (%) = [(Z-X) / (Y-X)] x 100

[0256] Furthermore, the pressure-sensitive adhesive sheets with release films produced in the Examples and Comparative Examples were cured by irradiating the pressure-sensitive adhesive sheets with light through the release film using a high-pressure mercury lamp so that the active energy rays having a wavelength of 365 nm achieved the integrated light amount shown in Table 3. Using the cured pressure-sensitive adhesive sheets, the gel fraction after curing was calculated in the same manner as the gel fraction before light irradiation.

[0257] [Adhesive Strength] The release film on one side of the adhesive sheet with release film prepared in the Examples and Comparative Examples was removed, and a PET film (Cosmoshine A4300, manufactured by Toyobo Co., Ltd., thickness 100 μm) was attached as a backing film using a hand roller. This was cut into strips 10 mm wide x 150 mm long, and the remaining release film was peeled off, and the exposed adhesive sheet surface was attached to the surface of soda lime glass using a hand roller. The resulting laminate was autoclaved (60 ° C, gauge pressure 0.2 MPa, 20 minutes) for finish attachment to prepare an adhesive strength measurement sample. The obtained adhesive strength measurement sample was peeled from the soda lime glass together with the backing film while being pulled at an angle of 180 ° at a peeling rate of 60 mm / min under conditions of 23 ° C, 50% RH, and the adhesive sheet was peeled off from the soda lime glass at an angle of 180 ° C, and the tensile strength (N / cm) was measured using a load cell to determine the adhesive strength.

[0258] [Adhesive strength after curing] The release film on one side was removed from the adhesive sheets with release film prepared in the Examples and Comparative Examples, and a PET film (Cosmoshine A4300, manufactured by Toyobo Co., Ltd., thickness 100 μm) was attached as a backing film using a hand roller. This was cut into strips 10 mm wide x 150 mm long, and the remaining release film was peeled off, and the exposed adhesive sheet surface was attached to the surface of soda lime glass using a hand roller. The resulting laminate was autoclaved (60 ° C, gauge pressure 0.2 MPa, 20 minutes) to finish adhesion. Thereafter, using a high-pressure mercury lamp, the adhesive sheet was irradiated with active energy rays having a wavelength of 365 nm through the backing film so that the accumulated light amount shown in Table 3 was obtained, and the adhesive sheet was cured to obtain an adhesive strength measurement sample. The obtained adhesive strength measurement sample was pulled at an angle of 180° at a peeling rate of 60 mm / min under conditions of 23°C and 50% RH, and the adhesive sheet together with the backing film was peeled off from the soda lime glass, and the tensile strength (N / cm) was measured with a load cell to determine the adhesive strength after curing.

[0259] [Bubble Resistance (Edge Bubble)] The pressure-sensitive adhesive sheets with release film prepared in the Examples and Comparative Examples were cut to 45 mm x 45 mm. The release film on one side of the cut pressure-sensitive adhesive sheet was removed, and the exposed adhesive surface was roll-pressed onto soda lime glass (54 mm x 82 mm x 0.6 mm thick). The remaining release film was then peeled off, and a polarizing plate (54 mm x 82 mm x 0.1 mm thick) was roll-laminated, followed by autoclaving (temperature 60 ° C, gauge pressure 0.8 MPa, 8 minutes) for finish lamination to produce a glass / pressure-sensitive adhesive sheet / polarizing plate laminate. The obtained laminate was irradiated from the soda lime glass side with an integrated light intensity of 365 nm at a wavelength of 3000 mJ / cm. 2 The adhesive sheet was irradiated with active energy rays using a metal halide lamp so that the edge bubble resistance (edge ​​bubble) was evaluated. Eight evaluation samples were prepared for each example. The number of bubbles generated within 1 mm from the edge of the adhesive sheet was counted, and the average number of edge bubbles per sample was calculated. An average number of bubbles of 10 or less was evaluated as "○ (good)", and an average number of bubbles greater than 10 was evaluated as "× (poor)".

[0260] [Adhesive Extrusion Resistance] The release film on one side of the adhesive sheets with release film produced in the Examples and Comparative Examples was peeled off and the sheets were half-cut to 10 mm x 10 mm. The exposed adhesive surface was placed opposite a 0.6 mm thick soda lime glass, and the adhesive sheet and glass were pressed together using a vacuum laminator at a temperature of 23°C, a gauge pressure of 0.4 MPa, and a pressure time of 60 seconds. The distance that the adhesive extruded from the half-cut marking line at the center of each side of the adhesive sheet was measured, and the average value of the four sides was taken as the adhesive extrusion distance (μm). Adhesive extrusion distances of 100 μm or less were evaluated as "Excellent", those of 200 μm or less were evaluated as "Good", and those of more than 200 μm were evaluated as "Poor".

[0261]

[0262] The pressure-sensitive adhesive sheets of the Examples had a stress relaxation rate (X0) of 0.20 or less and exhibited excellent end-face foaming resistance. This is thought to be because the excellent stress relaxation rate allowed gas trapped during lamination to escape easily, and any bubbles formed were easily eliminated over time. Furthermore, the pressure-sensitive adhesive sheets of Examples 1-1 to 1-7 also had excellent adhesive extrusion resistance because they had a predetermined initial elastic modulus (G0'(0)) value. On the other hand, the pressure-sensitive adhesive sheets of Comparative Examples 1-1 and 1-2 had a high stress relaxation rate (X0) and poor end-face foaming resistance. Furthermore, the pressure-sensitive adhesive sheet of Comparative Example 1-2 had a low storage shear modulus at 25°C (G'(25°C)) and exhibited poor adhesive extrusion resistance.

[0263] Example 2-1 100 parts by mass of an acrylic polymer (A-1), 1.5 parts by mass of a crosslinking agent (B-1), 2.45 parts by mass of a photoinitiator (C-1), 1.05 parts by mass of a photoinitiator (C-2), and 0.2 parts by mass of a silane coupling agent were prepared and uniformly mixed to form a pressure-sensitive adhesive composition for the front and back layers. On the other hand, 100 parts by mass of an acrylic polymer (A-4), 10 parts by mass of a crosslinking agent (B-2), and 1.0 part by mass of a photoinitiator (C-3) were prepared and uniformly mixed to form a pressure-sensitive adhesive composition for the intermediate layer. The pressure-sensitive adhesive composition for the front and back layers and the pressure-sensitive adhesive composition for the intermediate layer were each supplied to two extruders, and co-extruded into a two-kind, three-layer structure (outermost layer / intermediate layer / outermost layer, thickness ratio 1:4:1) to form a hot-melt sheet having a thickness of 150 μm. The sheet was sandwiched and laminated between two polyethylene terephthalate films (a PET film (thickness 100 μm) manufactured by Mitsubishi Chemical Corporation and a PET film (thickness 75 μm) manufactured by Mitsubishi Chemical Corporation) whose surfaces had been treated for release. Thereafter, the laminate was heated to 1500 mJ / cm using a high-pressure mercury lamp at a wavelength of 365 nm. 2 Both surfaces of the sheet-form pressure-sensitive adhesive composition were irradiated with active energy rays via the release film so as to obtain a pressure-sensitive adhesive sheet with a release film consisting of release film / pressure-sensitive adhesive sheet / release film. The pressure-sensitive adhesive sheet of Example 2-1 was a pressure-sensitive adhesive sheet equipped with active energy ray curability, which was cured by irradiation with active energy rays.

[0264] Examples 2-2 to 2-4 PSA sheets with release films were prepared in the same manner as in Example 2-1, except that the formulation, thickness ratio, and integrated light amount were changed to those shown in Table 4 below. The PSA sheets of Examples 2-2 to 2-4 were PSA sheets with active energy ray curability, which means that they were cured by irradiation with active energy rays.

[0265] Example 2-5 100 parts by mass of acrylic polymer (A-1), 1.5 parts by mass of crosslinking agent (B-1), 2.45 parts by mass of photoinitiator (C-1), 1.05 parts by mass of photoinitiator (C-2), and 0.2 parts by mass of silane coupling agent were prepared and uniformly mixed to prepare a pressure-sensitive adhesive composition.

[0266] Next, the pressure-sensitive adhesive composition was spread in a sheet form on a 100 μm-thick release film (a PET film manufactured by Mitsubishi Chemical Corporation) that had been subjected to a silicone release treatment so that the thickness of the pressure-sensitive adhesive composition was 150 μm. In addition, a 75 μm-thick release film (a PET film manufactured by Mitsubishi Chemical Corporation) that had been subjected to a silicone release treatment was laminated on the sheet-like pressure-sensitive adhesive composition. Thereafter, a high-pressure mercury lamp was used to irradiate the pressure-sensitive adhesive composition with an integrated light intensity of 500 mJ / cm at a wavelength of 365 nm. 2 Both surfaces of the sheet-form pressure-sensitive adhesive composition were irradiated with active energy rays via the release film so as to obtain a pressure-sensitive adhesive sheet with a release film consisting of release film / pressure-sensitive adhesive sheet / release film. The pressure-sensitive adhesive sheet of Example 2-5 was a pressure-sensitive adhesive sheet equipped with active energy ray curability, which was cured by irradiation with active energy rays.

[0267] Comparative Example 2-1 A pressure-sensitive adhesive sheet with a release film was produced in the same manner as in Example 2-1, except that the formulation, layer structure, and integrated light amount were changed to those shown in Table 4 below. The pressure-sensitive adhesive sheet of Comparative Example 2-1 was an active energy ray-curable pressure-sensitive adhesive sheet that was cured by irradiation with active energy rays.

[0268]

[0269] [Measurement and Evaluation of Physical Properties] The pressure-sensitive adhesive sheets produced in Examples 2-1 to 2-5 and Comparative Example 2-1 were subjected to the following various measurements and evaluations. The evaluation results are summarized in Table 5 below.

[0270] [Shear storage modulus (G')] The release film on one side was removed from the pressure-sensitive adhesive sheets with release films prepared in the Examples and Comparative Examples, and the sheets were repeatedly laminated with a hand roller to a thickness of approximately 0.9 mm, and then punched out into circles with a diameter of 9 mm to prepare samples. The obtained samples were placed in a rheometer ("DHR-2" manufactured by T.A. Instruments) and subjected to dynamic viscoelasticity measurement under the conditions of measurement jig: 8 mm diameter parallel plates, frequency: 1 Hz, measurement temperature: -50 to 150 ° C, and heating rate: 5 ° C / min, and the shear storage modulus (G') values ​​at 25 ° C and 85 ° C were read.

[0271] Furthermore, the pressure-sensitive adhesive sheets with release films prepared in the examples and comparative examples were subjected to irradiation with active energy rays having a wavelength of 365 nm using a metal halide lamp, with an integrated light intensity of 3000 mJ / cm 2 The pressure-sensitive adhesive sheet was irradiated with light through the release film to cure the pressure-sensitive adhesive sheet so that the shear storage modulus (G') of the cured pressure-sensitive adhesive sheet at 25°C and 85°C was measured using the cured pressure-sensitive adhesive sheet in the same manner as the shear storage modulus (G') before light irradiation.

[0272] [Glass transition temperature (Tg), Tanδ peak value] The release film on one side of the pressure-sensitive adhesive sheet with release film prepared in the Examples and Comparative Examples was removed, and the sheet was repeatedly laminated with a hand roller to a thickness of approximately 0.9 mm. A circle with a diameter of 9 mm was punched out to prepare a sample. The obtained sample was placed in a rheometer ("DHR-2" manufactured by T.A. Instruments) and subjected to dynamic viscoelasticity measurement under the following conditions: measurement jig: 8 mm diameter parallel plate; frequency: 1 Hz; measurement temperature: -50 to 150 ° C; heating rate: 5 ° C / min. From the Tanδ spectrum obtained by the dynamic viscoelasticity measurement, the temperature at which Tanδ reached its maximum value was read and designated as the glass transition temperature (Tg0). The maximum value is also shown in the table as the Tanδ peak value.

[0273] In addition, the pressure-sensitive adhesive sheets with release films prepared in the examples and comparative examples were irradiated with active energy rays having a wavelength of 365 nm using a metal halide lamp, with an integrated light intensity of 3000 mJ / cm 2 The adhesive sheet was irradiated with light through the release film to cure the adhesive sheet so that the glass transition temperature (Tg) of the cured adhesive sheet was measured using the cured adhesive sheet in the same manner as the glass transition temperature (Tg) before irradiation with light.

[0274] [Crossover Point Spacing (ΔT)] The release film on one side of the pressure-sensitive adhesive sheets with release film produced in the Examples and Comparative Examples was removed, and the sheets were repeatedly laminated with a hand roller to a thickness of approximately 0.9 mm, and then punched out into circles with a diameter of 9 mm to prepare samples. The obtained samples were placed in a rheometer ("DHR-2" manufactured by T.A. Instruments), and dynamic viscoelasticity measurements were performed under the following conditions: measurement jig: 8 mm diameter parallel plates, frequency: 1 Hz, measurement temperature: -50 to 150°C, and heating rate: 5°C / min. From the obtained dynamic viscoelasticity spectrum, the temperature (T1) at which the shear storage modulus (G') and loss modulus (G") become equal in the temperature range below the glass transition temperature (Tg0) was read. In addition, the temperature (T2) at which the shear storage modulus (G') and loss modulus (G") become equal in the temperature range above the glass transition temperature (Tg0) was read. The crossover point interval (ΔT) was calculated from the following formula: Crossover point interval (ΔT) = (T2) - (T1)

[0275] [Adhesive Strength] The release film on one side of the adhesive sheet with release film prepared in the Examples and Comparative Examples was removed, and a PET film (Cosmoshine A4300, manufactured by Toyobo Co., Ltd., thickness 100 μm) was attached as a backing film using a hand roller. This was cut into strips 10 mm wide x 150 mm long, and the remaining release film was peeled off, and the exposed adhesive sheet surface was attached to the surface of soda lime glass using a hand roller. The resulting laminate was autoclaved (60 ° C, gauge pressure 0.2 MPa, 20 minutes) for finish attachment to prepare an adhesive strength measurement sample. The obtained adhesive strength measurement sample was peeled from the soda lime glass together with the backing film while being pulled at an angle of 180 ° at a peeling rate of 60 mm / min under conditions of 23 ° C, 50% RH, and the adhesive sheet was peeled off from the soda lime glass at an angle of 180 ° C, and the tensile strength (N / cm) was measured using a load cell to determine the adhesive strength.

[0276] [Adhesion strength after curing] The release film on one side was removed from the pressure-sensitive adhesive sheets with release film prepared in the Examples and Comparative Examples, and a PET film (Cosmoshine A4300, manufactured by Toyobo Co., Ltd., thickness 100 μm) was attached as a backing film using a hand roller. This was cut into strips 10 mm wide x 150 mm long, and the remaining release film was peeled off, and the exposed pressure-sensitive adhesive sheet surface was attached to the surface of soda-lime glass using a hand roller. The obtained laminate was subjected to autoclave treatment (60°C, gauge pressure 0.2 MPa, 20 minutes) for finish attachment. Thereafter, a high-pressure mercury lamp was used to irradiate the sheet with an active energy ray having a wavelength of 365 nm until the cumulative light intensity was 3000 mJ / cm. 2 The adhesive sheet was irradiated with light through the backing film to cure the adhesive sheet, and used as an adhesive strength measurement sample. The adhesive strength measurement sample obtained was peeled off from the soda-lime glass together with the backing film while being pulled at an angle of 180° at a peeling rate of 60 mm / min under conditions of 23°C and 50% RH, and the tensile strength (N / cm) was measured with a load cell to determine the adhesive strength after curing.

[0277] [Bubble Resistance (Edge Bubble)] The pressure-sensitive adhesive sheets with release film prepared in the Examples and Comparative Examples were cut into 45 mm squares. The release film on one side of the cut pressure-sensitive adhesive sheet was removed, and the exposed adhesive surface was roll-pressed onto soda lime glass (52 mm x 84 mm x 0.6 mm thick). The remaining release film was then peeled off, and a polarizing plate (LJ01, 54 mm x 82 mm x 0.1 mm thick, manufactured by Shenzhen Qianhai Yuzhuo Technology Co., Ltd.) was roll-laminated, followed by autoclaving (temperature 60°C, gauge pressure 0.8 MPa, 8 minutes) for finish lamination to produce a glass / pressure-sensitive adhesive sheet / polarizing plate laminate. The obtained laminate was exposed to an integrated light intensity of 3000 mJ / cm at a wavelength of 365 nm from the soda lime glass side. 2The adhesive sheet was irradiated with active energy rays using a metal halide lamp so that the edge bubble resistance (edge ​​bubble) was evaluated. Ten evaluation samples were prepared for each example. The prepared samples were visually observed to confirm the number of bubbles generated within 1 mm from the edge of the adhesive sheet, and the average number of edge bubbles per sample was calculated. An average number of bubbles of 10 or less was evaluated as "○ (good)", and an average number of bubbles greater than 10 was evaluated as "× (poor)".

[0278]

[0279] The pressure-sensitive adhesive sheets of Examples 2-1 to 2-5 had a crossover point interval (ΔT) of 20°C or more between the shear storage modulus (G') and the loss modulus (G") in the dynamic viscoelasticity spectrum, and were excellent in end face foaming resistance. This is thought to be because, due to their excellent stress relaxation properties, gas taken in during lamination was easily released, and any bubbles that were formed were easily eliminated. On the other hand, the pressure-sensitive adhesive sheet of Comparative Example 2-1 had a narrow crossover point interval (ΔT), and was poor in end face foaming resistance.

[0280] Although the above examples show specific embodiments of the present invention, the examples are merely illustrative and should not be construed as limiting. Various modifications that are obvious to those skilled in the art are intended to fall within the scope of the present invention.

[0281] The pressure-sensitive adhesive sheet of the present invention has excellent lamination properties and can be laminated without air bubbles up to the peripheral edge near the edge of the pressure-sensitive adhesive sheet, and therefore can be suitably used as a pressure-sensitive adhesive sheet for image display devices, particularly image display devices with narrow frame designs or frameless designs.

Claims

1. A pressure-sensitive adhesive sheet having an acrylic pressure-sensitive adhesive layer formed from a pressure-sensitive adhesive composition containing an acrylic polymer (A), wherein the initial elastic modulus (G) of the acrylic pressure-sensitive adhesive layer after 0.1 seconds has elapsed since a strain of 25% was applied to the acrylic pressure-sensitive adhesive layer at a temperature of 70°C. 0 '(0)) and the relaxation modulus (G 0 The pressure-sensitive adhesive sheet has a stress relaxation rate (X0) calculated from the above formula (I) of 0.20 or less. 0 '(300) / G 0 '(0))...(I) 2. A pressure-sensitive adhesive sheet having an acrylic pressure-sensitive adhesive layer, the acrylic pressure-sensitive adhesive layer being a cured reaction product formed from a syrup composition containing an alkyl (meth)acrylate (a1) having an alkyl group with 3 to 30 carbon atoms, and a hydroxyl group-containing monomer (a2) and / or a nitrogen-containing monomer (a3), the initial elastic modulus (G) of the acrylic pressure-sensitive adhesive layer 0.1 seconds after applying a 25% strain at a temperature of 70°C is 0 '(0)) and the relaxation modulus (G 0 The pressure-sensitive adhesive sheet has a stress relaxation rate (X0) calculated from the above formula (I) of 0.20 or less. 0 '(300) / G 0 '(0))...(I) 3. The relaxation modulus (G 0 The pressure-sensitive adhesive sheet according to claim 1 or 2, wherein (0)′ is 5 to 100 kPa.

4. The relaxation modulus (G 0 The pressure-sensitive adhesive sheet according to claim 1 or 2, wherein the elastic modulus (300) is 0.1 to 20 kPa.

5. Shear storage modulus (G) at 25°C obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz 0 3. The pressure-sensitive adhesive sheet according to claim 1, wherein the compressive strength (MPa) (25° C.) is 100 kPa or more.

6. The glass transition temperature (Tg) defined by the maximum value of Tan δ obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz. 0 3. The pressure-sensitive adhesive sheet according to claim 1, wherein the temperature is -25° C. or higher.

7. The pressure-sensitive adhesive sheet according to claim 1 or 2, which is curable by active energy rays.

8. The pressure-sensitive adhesive sheet is exposed to active energy rays having a wavelength of 365 nm with an integrated light amount of 2000 to 4000 mJ / cm 2 The initial elastic modulus after curing (G 1 '(0)) and the post-curing relaxation modulus (G 1 The pressure-sensitive adhesive sheet according to claim 7, wherein the post-cure stress relaxation rate (X1) calculated from the above formula (II) is 0.22 or more. 1 '(300) / G 1 '(0))...(II) 9. The pressure-sensitive adhesive sheet according to claim 8, wherein the difference (X1-X0) between the post-cure stress relaxation rate (X1) and the stress relaxation rate (X0) is 0.01 or more.

10. The pressure-sensitive adhesive sheet is exposed to active energy rays having a wavelength of 365 nm with an integrated light amount of 2000 to 4000 mJ / cm 2 The initial elastic modulus after curing (G 1 The pressure-sensitive adhesive sheet according to claim 7, wherein the elastic modulus (0) is 1 kPa or more and 100 kPa or less.

11. The pressure-sensitive adhesive sheet is exposed to active energy rays having a wavelength of 365 nm with an integrated light amount of 2000 to 4000 mJ / cm 2 The post-curing relaxation elastic modulus (G 1 The pressure-sensitive adhesive sheet according to claim 7, wherein the elastic modulus (300) is 0.1 kPa or more and 50 kPa or less.

12. A pressure-sensitive adhesive sheet formed from a pressure-sensitive adhesive composition containing an acrylic polymer (A), which has a glass transition temperature (Tg) defined by the maximum value of Tan δ obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz. 0 ) is −40 to 20° C., 0 ) below which the shear storage modulus (G') and the loss modulus (G") become equal, and 0 ) or higher, the difference (ΔT) between the temperature (T2) at which the storage modulus (G') and the loss modulus (G") become equal is 20° C. or higher.

13. The pressure-sensitive adhesive sheet according to claim 12, wherein the maximum value of Tan δ is 1.2 or more.

14. The shear storage modulus (G 0 The pressure-sensitive adhesive sheet according to claim 12, wherein the compressive strength (MPa) (at 25°C) is 50 kPa or more.

15. The pressure-sensitive adhesive sheet according to claim 12, which is curable by active energy rays.

16. The pressure-sensitive adhesive sheet is exposed to active energy rays having a wavelength of 365 nm with an integrated light amount of 2000 to 4000 mJ / cm 2 The shear storage modulus (G) at a temperature of 25° C. obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz when irradiated so as to be 1 The pressure-sensitive adhesive sheet according to claim 15, wherein the compressive strength (MPa) (at 25°C) is 60 kPa or more.

17. The pressure-sensitive adhesive sheet is exposed to active energy rays having a wavelength of 365 nm with an integrated light amount of 2000 to 4000 mJ / cm 2 The shear storage modulus (G) at a temperature of 85° C. obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz when irradiated so as to be 1 The pressure-sensitive adhesive sheet according to claim 15, wherein the compressive strength (MPa) (85° C.) is 10 kPa or more.

18. The pressure-sensitive adhesive sheet according to any one of claims 1, 2 and 12, having a gel fraction of 30 to 90%.

19. The pressure-sensitive adhesive sheet according to any one of claims 1, 2 and 12, wherein the pressure-sensitive adhesive composition or syrup composition contains a crosslinking agent (B) and / or a photoinitiator (C).

20. An adhesive sheet according to any one of claims 1, 2 and 12, wherein the adhesive composition or syrup composition contains a photoinitiator (C), the photoinitiator (C) including a photoinitiator (c1) having within its molecule a radically polymerizable functional group having a carbon-carbon double bond and a structure that generates radicals, and a hydrogen abstraction type photoinitiator (c2) other than the photoinitiator (c1).

21. The pressure-sensitive adhesive sheet according to claim 1 or 12, wherein the acrylic polymer (A) has a structural unit derived from a nitrogen-containing monomer (a3).

22. An adhesive sheet with a release film, comprising the adhesive sheet according to any one of claims 1, 2 and 12, and a release film laminated on the adhesive sheet.

23. A laminate for an image display device comprising two image display device components and an adhesive sheet described in any one of claims 1, 2 or 12 interposed between the two image display device components, one of the two image display device components being a surface protection panel and the other being a member consisting of any one or a combination of two or more of the group consisting of a touch sensor film, an image display panel, a color filter, a polarizing element and a retardation film.

24. The laminate for an image display device according to claim 23, wherein the surface protection panel has a frame-shaped concealing portion on the periphery, and has a portion where the frame width is 3 mm or less.

25. The laminate for an image display device according to claim 23, which is fixed in a curved shape.

26. An image display device comprising the laminate for an image display device according to claim 23.

27. An adhesive sheet for use as a component of an image display device, comprising the adhesive sheet according to any one of claims 1, 2 and 12.

Citation Information

Patent Citations

  • Pressure-sensitive adhesive sheet, method of manufacturing laminate and laminate

    JP2019077747A

  • Adhesive sheet and production method of the same, and method for manufacturing image display device

    JP2019131679A

  • Photocurable pressure-sensitive adhesive sheet laminate, method for manufacturing photocurable pressure-sensitive adhesive sheet laminate, and method for manufacturing image display panel laminate

    JP2019210446A

  • Adhesive sheet, laminated sheet and flexible image display device

    JP2023038851A

  • Adhesive Composition and Adhesive Sheet Using the Same

    KR102229885B1

Cited By

  • Laminate for constituting image display device, method for manufacturing same, and image display device constituent member with release film

    WO2026204932A1