Polishing pad and production method therefor

By embedding fiber materials within the resin of polishing pads, the strength of convex portions is enhanced, addressing the issue of peeling and deformation, and resulting in a more durable and effective polishing surface with increased bending strength.

WO2024203830A1PCT designated stage expired Publication Date: 2024-10-03FUJIBO HLDG
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011258
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Polishing pads with concavo-convex patterns formed using intaglio methods often face issues with the convex portions peeling off during manufacturing and polishing due to insufficient strength, leading to damage and deformation.

Method used

Incorporating a fiber material within the resin of the polishing pad, which is integrally molded with the convex and base portions, enhances the strength of the convex parts, preventing them from falling off during peeling and polishing, and using a method that involves preparing an intaglio plate, embedding a sheet-like fibrous material in the resin before curing, and peeling off the cured resin to obtain the polishing layer.

Benefits of technology

The embedded fiber material increases the bending strength of the polishing layer to 30 MPa or more, reducing damage and deformation during peeling and polishing, and ensures the convex portions remain intact, improving the pad's durability and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011258_03102024_PF_FP_ABST
    Figure JP2024011258_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a polishing pad obtained by a method in which, when a rugged pattern is transferred to a resin 50 using an intaglio plate 72, protrusions 51 of the resin 50 are less apt to fall off, the protrusions 51 having excellent strength. Disclosed is a polishing pad having a polishing layer 11 comprising protrusions 51 and a base 52 provided beneath the protrusions 51. The polishing pad is characterized in that the protrusions 51 and the base 52 were of the polishing layer 11 have been integrally molded from the same resin 50 and that the base 52 has a fibrous material 6 embedded therein.
Need to check novelty before this filing date? Find Prior Art

Description

Polishing pad and method of manufacturing the same

[0001] The present invention relates to a polishing pad and a method for manufacturing the same. In particular, the polishing pad of the present invention is used for lapping and polishing optical materials, semiconductor devices, glass substrates for hard disks, etc., and is particularly suitable for lapping and polishing sapphire, SiC, etc.

[0002] Polishing pads are used for lapping and polishing optical materials, semiconductor devices, glass substrates for hard disks, sapphire, and SiC. Various types of polishing pads are known, including polishing pads using nonwoven fabric, polishing pads using foamed or non-foamed polyurethane, polishing pads with fixed abrasive grains, and polishing pads using a resin layer with a concave-convex pattern as the polishing surface.

[0003] Among these, the polishing pad using a resin layer having a concave-convex pattern as the polishing surface has the advantage that the grooves forming the concave-convex pattern affect the fluidity of the slurry, and as a result, the object to be polished can be polished uniformly. The manufacturing method of such a polishing pad includes a method of cutting the surface of a flat base material to form grooves, a method of forming a concave-convex pattern on a substrate by applying a screen printing method, and a method of making a mold having a concave-convex pattern and using the mold to mold.

[0004] For example, Patent Document 1 discloses a polishing pad (C50) on which a concave-convex pattern is formed by transferring from a plate (C72 in FIG. 1) having a concave-convex pattern made of photosensitive resin, and Patent Document 2 discloses a polishing pad on which a concave-convex pattern is formed using a mold made of silicone rubber or the like onto which a plate having a concave-convex pattern made of photosensitive resin is transferred. However, the methods of transferring a concave-convex pattern to a resin using an intaglio plate as in Patent Documents 1 and 2 have problems such as difficulty in peeling the cured resin from the intaglio plate, and the protrusions (C51) of the resin are cut (C9), causing the protrusions (C51) to fall off (see FIGS. 1 and 2).

[0005] JP 2019-178248 JP 2019-178258

[0006] The present invention has been made in consideration of the above problems, and provides a polishing pad having a polishing layer with excellent convex strength, so that the convex portions of the resin are less likely to fall off when a concave-convex pattern is transferred to the resin using an intaglio printing plate, and a method for manufacturing the same.

[0007] As a result of investigations, the inventors have discovered a polishing pad in which the strength of the convex portions is increased by providing a fibrous material inside the resin of the base, thereby preventing the convex portions of the polishing pad from falling off during manufacturing (when peeling from the intaglio) and polishing. The present invention encompasses the following: [1] A polishing pad having a polishing layer consisting of convex portions and a base portion provided below the convex portions, wherein the convex portions and the base portion of the polishing layer are integrally molded from the same resin, and a fibrous material is embedded in the base. [2] The polishing pad described in [1], wherein the resin is a curable resin composition. [3] The polishing pad described in [1], wherein the fibrous material is a woven fabric. [4] The polishing pad described in [1], wherein the fiber diameter of the fibrous material is 100 μm or more and 300 μm or less. [5] The polishing pad described in [1], wherein the mesh size of the fibrous material is 10 μm or more and 700 μm or less. [6] The polishing pad described in [1], wherein the average height of the convex portions is 0.3 mm or more and 1.5 mm or less. [7] The polishing pad according to [1], wherein the convex portions have a shape of a truncated quadrangular pyramid. [8] A method for manufacturing a polishing pad having a polishing layer formed by curing a resin and having convex portions, the method comprising the steps of: preparing an intaglio plate having a concave-convex pattern; pouring a resin raw material into the intaglio plate; embedding a sheet-like fiber material in the resin before the resin hardens; hardening the resin; and peeling the hardened resin from the intaglio plate to obtain the polishing layer. [9] The polishing pad according to [8], wherein the polishing layer comprises the convex portions and a base portion provided below the convex portions, and the convex portions and the base portion are integrally molded from the same resin.

[10] The polishing pad according to [8], wherein the fiber material is a woven fabric.

[11] The polishing pad according to [8], wherein the resin is a photocurable resin.

[12] A method for manufacturing a polishing pad having a polishing layer formed by curing a resin and having convex portions, the method comprising the steps of: preparing an intaglio plate having a concave-convex pattern; arranging a sheet-like fiber material on the intaglio plate; pouring a resin raw material into the intaglio plate with the fiber material arranged on it; curing the resin; and peeling the cured resin from the intaglio plate to obtain the polishing layer.

[0008] A polishing pad in which the convex portions and base portion are integrally molded from the same resin, the base portion has a concave-convex pattern, and a fiber material is embedded in the resin inside, has increased strength in the convex portions, and can prevent the convex portions from falling off during manufacturing (when peeling off from the intaglio) and polishing. By embedding a fiber material inside the resin, the strength of the convex portions of the polishing layer is increased, and can prevent the convex portions of the polishing layer from falling off during manufacturing (when peeling off from the intaglio) and polishing.

[0009] Fig. 1 is a process diagram of a conventional method for manufacturing a polishing layer. Fig. 2 is a schematic diagram illustrating damage and falling off C9 of convex portions C51 when a conventional polishing layer is peeled off from an intaglio C72. Fig. 3 is a cross-sectional view of the polishing layer 11 of the polishing pad of the present invention. Fig. 4 is a process diagram of the method for manufacturing the polishing layer 11 of the polishing pad of the present invention. Fig. 5 is a photograph of the polishing layer of Example 1. Fig. 6 is a cross-sectional view of the polishing layer 11 of the polishing pad of the present invention, which is another embodiment.

[0010] The following describes the form for carrying out the invention, but the present invention is not limited to the form for carrying out the invention, and various modifications are possible within the scope that does not deviate from the gist of the invention.

[0011] <<Polishing Pad>> As shown in Figure 3, the polishing pad of the present invention has a polishing layer 11 consisting of convex portions 51 on the upper surface and a base portion 52 provided below the convex portions 51, in which the convex portions 51 and the base portion 52 of the polishing layer 11 are integrally molded from the same resin 50, and the polishing layer 11 has a concave-convex pattern due to the presence of multiple convex portions 51, and a fibrous material 6 is embedded in the resin 50 of the base portion 52. Note that in this specification, embedding a fibrous material in a resin refers to inserting all or part of the fibrous material into the resin. For convenience, both the resin raw material before pouring into a mold (i.e., the resin before hardening) and the hardened resin will be represented by the symbol 50.

[0012] The resin 50 is not particularly limited as long as a resin layer 11 having convex portions 51 is obtained, but a curable resin composition is preferred. The curable resin composition is not particularly limited, but examples thereof include thermosetting resins; UV-curable resins; photocurable resin compositions containing a photopolymerization initiator and a polymerizable compound; thermosetting resin compositions containing a thermal polymerization initiator and a polymerizable compound; and curable resin compositions containing a two-component mixed curable resin. Furthermore, the curable resin composition may contain a crosslinking agent having two or more polymerizable functional groups, if necessary.

[0013] The thermosetting resin is not particularly limited, but examples thereof include phenol resin, epoxy resin, acrylic resin, urethane resin, and formaldehyde resin.

[0014] The UV-curable resin is not particularly limited, but for example, a prepolymer having a number-average molecular weight of about 1,000 to 10,000 is preferable, and examples of the material include isocyanurate-based resins, acrylic (methacrylic) ester resins and urethane-modified resins thereof, and thiokol-based resins, and a reactive diluent or organic solvent can be used as appropriate depending on the application.

[0015] Examples of photopolymerization initiators include benzophenone compounds, acetophenone compounds, and thioxanthone compounds. Examples of thermal polymerization initiators include azo compounds such as 2,2'-azobisbutyronitrile, and peroxides such as methyl ethyl ketone peroxide and benzoyl peroxide (BPO).

[0016] Specific examples of the resin include unsaturated carboxylic acids having a polymerizable unsaturated group, such as (meth)acrylic acid, itaconic acid, crotonic acid, isocrotonic acid, and maleic acid; unsaturated carboxylic acid esters having a polymerizable unsaturated group, such as (meth)acrylate, epoxy (meth)acrylate (vinyl ester resin), urethane (meth)acrylate, and polyester (meth)acrylate; polyesters having an unsaturated group; polyethers having a polymerizable unsaturated group; polyamides having a polymerizable unsaturated group; urethanes having a polymerizable unsaturated group; and aromatic compounds having a polymerizable unsaturated group, such as styrene.

[0017] The two-component mixed curable resin is not particularly limited, but examples thereof include prepolymers with different physical properties, such as epoxy resin, unsaturated polyester resin, and polyamide resin.

[0018] Among these, those that cure at room temperature are preferred, from the viewpoints of being easily cured into the desired shape and of the heat resistance of the intaglio 72. Such curable resin compositions are not particularly limited, but examples include curable resin compositions containing a polymerization initiator that acts at room temperature, UV-curable resin compositions and photocurable resin compositions that cure upon exposure to light, and mixed curable resin compositions that cure by mixing two liquids. Furthermore, in terms of polishing (lapping) performance, vinyl ester resins or unsaturated polyester resins, which have high heat resistance (high deformation temperature), are preferred.

[0019] The flexural strength of the abrasive layer 11 is 30 MPa or more, preferably 30 to 1000 MPa, more preferably 40 to 900 MPa, and even more preferably 50 to 800 MPa. The flexural strength is obtained by measurement performed in accordance with JIS K7203. When the flexural strength is within the above range, damage or deformation of the abrasive layer 11 can be suppressed when the abrasive layer 11 is peeled off from the intaglio 72.

[0020] Furthermore, it is preferable that the polishing layer 11 comprises a convex portion 51 and a base portion 52 provided below the convex portion 51, the base portion 52 and the convex portion 51 being integrally molded from the same resin and having a concave-convex pattern. By integrally molding the convex portion 51 and the base portion 52, the process of joining the convex portion 51 and the base portion 52 is eliminated, thereby reducing costs. Furthermore, the joining strength is higher than when the convex portion 51 and the base portion 52 are bonded, making it more difficult for the convex portion 51 to come off the base portion 52.

[0021] The fiber material 6 may be positioned so as to be in contact with the protrusions 51 (i.e., the part of the base 52 closest to the protrusions 51), or may be positioned so as to be farthest from the protrusions 52 (i.e., near the surface opposite the protrusions 51), but it is preferable to position the fiber material 6 at a position approximately at the center of the height direction of the base 52. This is because this makes manufacturing easier and also increases the strength of the protrusions 51.

[0022] The fibrous material 6 embedded in the resin 50 of the base 52 of the polishing layer 11 of the polishing pad may be in the form of threads, bundles, cotton, cloth, etc., with cloth being preferred. Examples of cloth-like fibrous materials include woven fabrics, knitted fabrics, and nonwoven fabrics. To enhance resin strength, woven fabrics and knitted fabrics are preferred, with mesh fabrics being particularly preferred. Materials for the fibrous material 6 include organic fibers, inorganic fibers, synthetic fibers, semi-synthetic fibers, recycled fibers, etc. Examples of organic fibers include, but are not limited to, fibers derived from natural sources such as cellulose, carbon fiber, pulp, chitin, and chitosan. Examples of inorganic fibers include, but are not limited to, glass fiber, rock fiber, and metal fiber. Examples of synthetic fibers include, but are not limited to, nylon, vinylon, vinylidene, polyester, polyolefins (e.g., polyethylene, polypropylene, etc.), polyurethane, acrylic, polyvinyl chloride, and aramid. Examples of semi-synthetic fibers include, but are not limited to, acetate, triacetate, and promix. Examples of recycled fibers include, but are not limited to, rayon, cupra, polynosic rayon, lyocell, Tencel, etc. The fiber material 6 embedded in the resin 50 of the base 52 of the polishing layer 11 of the polishing pad of the present invention is preferably polyethylene or polypropylene from the viewpoints of ease of availability and ease of processing.

[0023] The fiber diameter of the fiber material 6 is 100 μm or more and 300 μm or less, more preferably 150 μm or more and 250 μm or less. When the fiber diameter of the fiber material 6 is within the above range, it functions as a skeleton material for the resin 50 and can increase the strength of the polishing layer 11. If the fiber diameter is less than 100 μm, the strength may be insufficient, and if the fiber diameter is more than 300 μm, air may get in from the surroundings when the fiber is incorporated into the resin 50.

[0024] The mesh size of the fiber material 6 is 10 μm or more and 700 μm or less, more preferably 30 μm or more and 520 μm or less. When the mesh size of the fiber material 6 is within the above range, the fiber material 6 can be appropriately incorporated into the polishing layer 11, thereby increasing the strength of the resin 50. If the mesh size is less than 10 μm, the resin 50 will not be easily absorbed, and if the mesh size is more than 700 μm, the resin 50 will not function as a skeletal material, resulting in insufficient strength.

[0025] The thickness of the fiber material 6 is 100 μm or more and 500 μm or less, more preferably 150 μm or more and 300 μm or less. When the thickness of the fiber material 6 is within the above range, the strength of the resin 50 can be increased without impairing the polishing performance of the polishing pad.

[0026] The average height of the convex portions 51 of the uneven pattern of the polishing layer 11 of the polishing pad of the present invention is preferably 0.3 mm or more and 1.5 mm or less, and more preferably 0.8 mm or more and 1.2 mm or less. If the average height of the convex portions 51 is less than 0.3 mm, the product life (life) of the polishing pad will be shortened, and if it is greater than 1.5 mm, there is a risk of the convex portions 51 falling off or being damaged during production. In this specification, the height of the convex portions 51 is defined as α in FIG. 3 (the distance from the surface of the base 52 facing the convex portions 51 to the highest point of the convex portions 51). That is, it is the distance from the part of the convex portions 51 that contacts the base 52 to the top end of the convex portions 51. In this example, the shape of the convex portions 51 of the polishing layer 11 is a truncated quadrangular pyramid, but it may also be a truncated cone shape such as a truncated cone, an approximately truncated cone, or an elliptical truncated cone, or a columnar shape such as a square pillar, a cylinder, an approximately cylindrical cylinder, or an elliptical cylinder.

[0027] <<Method for Manufacturing Polishing Pad>> A first aspect of the method for manufacturing a polishing pad of the present invention is as follows: That is, the method for manufacturing a polishing pad has a polishing layer 11 formed by curing a resin 50 and having convex portions 51, and includes the steps of: preparing an intaglio 72 having a concave-convex pattern (Step 1); pouring a resin raw material 50 into the intaglio 72 (Step 2); embedding a sheet-like fiber material 6 in the resin 50 before the resin 50 hardens (Step 3); hardening the resin 50 (Step 4); and peeling the hardened resin 50 from the intaglio 72 to obtain the polishing layer 11 (Step 5).

[0028] In this specification, embedding a fiber material in a resin refers to inserting all or part of the fiber material into the resin. Figure 1 shows a flowchart of a conventional method for manufacturing a polishing layer, and Figure 4 shows a flowchart of a method for manufacturing a polishing layer 11 of a polishing pad (first embodiment) of the present invention. The following explanation will mainly be given based on Figure 4.

[0029] (Step 1) An intaglio plate 72 having a concave-convex pattern formed thereon is prepared. The intaglio plate 72 having a concave-convex pattern formed thereon may be a mold having a concave-convex pattern, an intaglio plate made of a photosensitive resin, an intaglio plate made of silicone rubber or the like, an intaglio plate made of a plastic material, or the like, and is not particularly limited as long as it can obtain a polishing layer 11 having convex portions 51 formed on its upper surface. Note that an intaglio plate is a plate that provides concave portions on the surface into which the resin is poured, thereby allowing convex portions to be formed in the resin material.

[0030] Note that a step of applying a release agent to the intaglio 72 may be performed before pouring the resin raw material 50 into the intaglio 72. The release agent is not particularly limited as long as it can peel the cured resin from the intaglio 72, and examples thereof include silicone-based release agents and fluorine-based release agents, with fluorine-based release agents being preferred. The method of applying the release agent is not particularly limited as long as it can peel the cured resin from the intaglio 72, and examples thereof include spraying and electrostatic application, with spraying being preferred.

[0031] (Step 2) The resin raw material 50 is poured into the intaglio 72. The method for pouring the resin raw material 50 into the intaglio 72 is not particularly limited as long as it allows the resin raw material 50 to be filled (pouring) into the recesses of the intaglio 72. Examples include gravity casting, in which the resin raw material is poured into the recesses under its own weight at room temperature and normal pressure, and vacuum casting, in which the intaglio 72 and resin 50 are placed in a vacuum container, the pressure is reduced, and the resin 50 is poured into the recesses at atmospheric pressure. When pouring the resin 50, because the polishing layer 11 has the convex portions 51 and the base 52, it is necessary to pour the resin 50 not only into the recesses of the intaglio 72, but also to a height that exceeds the height of the convex portions of the intaglio 72 to form the base 52.

[0032] (Step 3) A process of embedding a sheet-like fiber material 6 in the resin 50 before the resin 50 hardens will be described. The method of embedding the sheet-like fiber material 6 in the resin 50 before the resin 50 hardens is not particularly limited as long as it can embed the fiber material 6 in the resin 50. For example, a method is conceivable in which the resin 50 is poured into an intaglio 72, and then the sheet-like fiber material 6 is placed in the resin 50 in a low-viscosity state before hardening, and the fiber material 6 is embedded in the resin 50 by applying pressure under its own weight or by hand. The positional relationship between the fiber material 6 and the intaglio 72 may be such that the fiber material 6 does not contact the uneven pattern of the intaglio 72, as shown in FIG. 4 , or such that the fiber material 6 contacts the uneven pattern of the intaglio 72.

[0033] The timing for embedding the fiber material 6 in the resin 50 may be during or after the process of pouring the resin raw material 50 into the intaglio 72, but is not particularly limited as long as it is possible to embed it in the resin 50, and varies depending on the materials and strength adjustments of the resin raw material 50 and the fiber material 6.

[0034] Furthermore, after embedding the fiber material 6 in the resin 50, and before curing the resin 50, a step of bonding a substrate to the surface of the resin 50 opposite to the surface that contacts the intaglio 72 may be further included. By using a substrate, the resin 50 is cured in a state where it is sandwiched between the substrate and the intaglio 72. This tends to improve the uniformity of the thickness of the obtained cured product and further improve the flatness of the back surface (the surface opposite to the surface that contacts the intaglio 72) of the obtained cured product.

[0035] (Step 4) The process of curing the resin raw material 50 will be described. The method of curing the resin raw material 50 is not particularly limited as long as it is a method suitable for each resin raw material 50, and examples thereof include a photocuring method in which ultraviolet light or the like is irradiated, a thermal curing method in which heat is applied (including a method in which the material is left at room temperature), or a method in which the material is mixed and left to stand, such as a two-liquid mixing type. Examples of the device used include a method using a light irradiating device or a method using a thermostatic device. The light irradiating device is not particularly limited as long as it is a device that emits light in a wavelength range that includes the wavelength of light at which the photocurable resin cures, and examples thereof include an ultraviolet irradiating device. The light to be irradiated is not particularly limited as long as it is capable of curing the resin raw material 50, and examples thereof include ultraviolet light. Examples of light sources that emit such light include high-pressure mercury lamps, UV-LED lamps, and black light fluorescent lamps (BLBs). Among these, BLBs are preferred. The light irradiation direction may be from either the lower surface 72A of the plastic intaglio 72 or the upper surface 50A of the resin raw material 50. Irradiation from the lower surface 72A allows sufficient light to reach the convex portions 51, resulting in sufficient curing of the convex portions 51. The wavelength of the ultraviolet irradiation is preferably 200 nm to 400 nm, and the irradiation time is preferably 3 minutes to 30 minutes. Examples of heat-curing methods include placing the intaglio 72 with the resin raw material 50 poured into it in an oven and heating it, or preheating the intaglio 72 and then pouring the resin raw material 50 into it. The resin raw material 50 is preferably cured after the fiber material 6 is embedded in the uncured resin 50.

[0036] (Step 5) The cured resin 50 is peeled off from the intaglio 72 to obtain the polishing layer 11. The peeling method may involve holding the edge of the polishing layer 11 and peeling it off from the intaglio 72. The resulting polishing layer 11 has a concave-convex pattern transferred from the intaglio 72, and the surfaces of the convex portions 51 of the concave-convex pattern become the polishing surface for polishing the workpiece.

[0037] The resulting abrasive layer 11 has a bending strength of 30 MPa or more, preferably 30 to 1000 MPa, more preferably 40 to 900 MPa, and even more preferably 50 to 800 MPa. The bending strength is obtained by measurement performed in accordance with JIS K7203. When the bending strength is within the above range, breakage or deformation of the abrasive layer 11 can be suppressed when the abrasive layer 11 is peeled off from the intaglio 72.

[0038] Furthermore, it is preferable that the polishing layer 11 comprises a convex portion 51 and a base portion 52 provided below the convex portion 52, and the base portion 52 and the convex portion 51 are integrally molded from the same resin and have a concave-convex pattern. By integrally molding the convex portion 51 and the base portion 52, the process of joining the convex portion 51 and the base portion 52 is eliminated, thereby reducing costs. Furthermore, the bonding strength is higher than when the convex portion 51 and the base portion 52 are bonded, making it difficult for the convex portion 51 to come off the base portion 52. The surface of the polishing layer 11 with the convex portion 51 becomes the polishing surface.

[0039] Next, a second embodiment of the manufacturing method of the present invention will be described. The second embodiment is as follows: A method for manufacturing a polishing pad having a polishing layer 11 formed by curing a resin 50 and having protrusions 51, the method comprising the steps of: preparing an intaglio 72 having a concave-convex pattern; arranging a sheet-like fiber material 6 on the intaglio 72; pouring a resin raw material 50 into the intaglio 72 with the fiber material 6 disposed thereon; curing the resin 50; and peeling the cured resin 50 from the intaglio 72 to obtain the polishing layer 11.

[0040] The second embodiment has many parts in common with the first embodiment, but in the second embodiment, the sheet-like fiber material 6 is placed before the resin 50 is poured into the intaglio 72, and then the resin 50 is poured in. By doing so, it is not necessary to embed the sheet-like fiber material 6, but it is necessary to prevent the sheet-like fiber material 6 from being washed away when the resin 50 is poured in.

[0041] When the sheet-like fiber material 6 has openings such as a mesh fabric, the second embodiment is preferably used.

[0042] FIG. 6 shows a polishing layer 11 having a different shape from that shown in FIG. 3 . The polishing layer 11 differs from the polishing layer 11 shown in FIG. 6 in that it includes a recess 53 on the opposite side of the protrusion 51. By including the recess 53, further weight reduction and cost reduction can be achieved. The recess 53 can be formed by intentionally reducing the amount of resin in the area where the protrusion 51 is to be formed in Step 2, or by pressing a mold corresponding to the recess 53 from above after Step 3. The shape of the recess 53 is not particularly limited, and may be a shape with corners (e.g., a truncated pyramid) as shown in FIG. 6 or a shape with a curved surface (e.g., a dome shape).

[0043] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0044] In each example and comparative example, unless otherwise specified, "parts" means "parts by mass."

[0045] (Manufacturing of polishing pads)

[0046] (Production of Polishing Pad 1) A polypropylene resin sheet was vacuum-formed to produce an intaglio 72 having multiple truncated pyramidal recesses with a height of 0.85 mm and bases of 1.5 mm square. Next, 90 parts of unsaturated polyester resin (product name: Rigolac, manufactured by Resonac Co., Ltd.) was poured into the intaglio 72. Before curing, a mesh fabric made of polypropylene with a fiber diameter of 150 μm, a mesh size of 30 μm, and a thickness of 300 μm was sunk into the resin 50 from above, allowing the fiber material 6 to penetrate into the base 52. The resin 50 was cured at room temperature (25°C) for 30 minutes, and then the intaglio 72 was removed by peeling the resin 50 from the intaglio 72, thereby producing the polishing pad 1.

[0047] (Manufacture of Polishing Pad 2) Polishing pad 2 was manufactured in the same manner as polishing pad 1, except that the polishing pad material was made of vinyl ester resin (product name: Lipoxy, manufactured by Resonac Co., Ltd.) instead of unsaturated polyester resin, and the mesh fabric material was made of polyethylene fiber instead of polypropylene fiber.

[0048] Furthermore, in manufacturing polishing pad 2, it was confirmed that even if the material of the polishing pad and the material of the mesh fabric were changed, a polishing pad similar to polishing pad 1 could also be manufactured using a plastic intaglio made of polypropylene resin.

[0049] (When peeling from the intaglio plate) A peeling experiment was conducted to peel the resin 50 from the intaglio plate 72 using a peeling roller. Examples of the peeling roller include a combination of adhesive tape and a rod-shaped peeling roller, as described in JP-A-9-114384. Peeling experiments were conducted under conditions that allowed peeling of the intaglio plate 72 and the resin 50, using the base 52 containing the mesh fabric according to the above example and the base 52 not containing the mesh fabric. When the intaglio plate 72 not containing the mesh fabric experienced damage or loss of the protrusions 51, the polishing pad 1 and polishing pad 2 obtained using the plastic intaglio plate 72 made of polypropylene resin did not experience any damage or loss of the protrusions 51 during peeling (see the photograph in FIG. 5).

[0050] The present invention provides a polishing pad in which the strength of the convex portion 51 is increased and the polishing pad convex portion 51 can be prevented from falling off during manufacturing (when peeling from the intaglio 72) and polishing, thereby contributing to the manufacture and sale of polishing pads and having industrial applicability.

[0051] 11 Polishing layer 72 Intaglio 72A Intaglio lower surface 50 Resin raw material 50A Resin raw material upper surface 51 Convex portion 52 Base portion 53 Concave portion 6 Fiber material C9 Damage and detachment of convex portion

Claims

1. A polishing pad having a polishing layer consisting of a convex portion and a base portion provided below the convex portion, wherein the polishing layer has a convex portion and a base portion integrally molded from the same resin, and a fibrous material is embedded in the base portion.

2. The polishing pad of claim 1, wherein the resin is a curable resin composition.

3. The polishing pad of claim 1, wherein the fibrous material is a woven fabric.

4. The polishing pad according to claim 1, wherein the fiber diameter of the fiber material is 100 μm or more and 300 μm or less.

5. The polishing pad according to claim 1, wherein the opening of said fiber material is 10 μm or more and 700 μm or less.

6. The polishing pad according to claim 1, wherein the average height of said convex portions is 0.3 mm or more and 1.5 mm or less.

7. The polishing pad according to claim 1, wherein the shape of said convex portion is a truncated pyramid.

8. A method for manufacturing a polishing pad having a polishing layer formed by hardening a resin and having convex portions, comprising the steps of: preparing an intaglio plate having a concave-convex pattern; pouring a resin raw material into the intaglio plate; embedding a sheet-shaped fiber material in the resin before the resin hardens; hardening the resin; and peeling the hardened resin from the intaglio plate to obtain the polishing layer.

9. A method for manufacturing a polishing pad as described in claim 8, wherein the polishing layer comprises the convex portion and a base portion provided below the convex portion, and the convex portion and the base portion are integrally molded from the same resin.

10. The method of claim 8, wherein the fibrous material is a woven fabric.

11. The method for producing a polishing pad according to claim 8, wherein the resin is a photocurable resin.

12. A method for manufacturing a polishing pad having a polishing layer formed by hardening a resin and having convex portions, comprising the steps of: preparing an intaglio plate having a concave-convex pattern; arranging a sheet-like fibrous material on the intaglio plate; pouring a resin raw material into the intaglio plate with the fibrous material arranged thereon; hardening the resin; and peeling the hardened resin from the intaglio plate to obtain the polishing layer.

Citation Information

Patent Citations

  • Abrasive ground fabric and manufacturing method thereof

    JP1986079575A

  • Abrasive article, and its manufacture

    JP1993253849A

  • abrasive brushes and filaments

    JP2001502185A

  • Polishing pad for chemical mechanical polishing (CMP), and its manufacturing method

    JP2004306195A

  • Abrasive pad and method for manufacturing the same, and method for manufacturing polished product