Method for producing polishing pad

The use of disposable plastic intaglio plates with low surface free energy materials and mold release agents addresses the challenges of peeling and durability in polishing pad manufacturing, enabling cost-effective and durable polishing pads for optical and semiconductor applications.

WO2024203831A1PCT designated stage expired Publication Date: 2024-10-03FUJIBO HLDG
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011259
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing methods for manufacturing polishing pads with concavo-convex patterns using intaglio plates face challenges such as difficulty in peeling off the cured resin, high costs, and poor durability of materials like photosensitive resin and silicone rubber, making them unsuitable for mass production.

Method used

A method using a disposable plastic intaglio plate made from general-purpose plastic with low surface free energy materials like polyolefins or polystyrene, combined with a mold release agent, to easily peel off the resin and form a polishing layer with a concavo-convex pattern, reducing costs and improving durability.

Benefits of technology

This method allows for the cost-effective production of polishing pads with easily removable resin layers, preventing damage during peeling and enhancing the durability of the polishing pads, making them suitable for mass production and effective in polishing optical materials and semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011259_03102024_PF_FP_ABST
    Figure JP2024011259_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a method for producing a polishing pad, wherein, when a rugged pattern is transferred onto a resin using an intaglio plate, the resin can be easily peeled at low cost. Disclosed is a method for producing a polishing pad having a polishing layer obtained by curing a resin, the method comprising: a step for preparing a plastic intaglio plate having a textured pattern formed by vacuum molding or injection molding; a step for pouring a resin material onto the plastic intaglio plate; a step for curing the resin; and a step for peeling the cured resin from the plastic intaglio plate to obtain the polishing layer.
Need to check novelty before this filing date? Find Prior Art

Description

Polishing pad manufacturing method

[0001] The present invention relates to a polishing pad. In particular, the polishing pad of the present invention is used for lapping and polishing optical materials, semiconductor devices, glass substrates for hard disks, etc., and is particularly suitable for lapping and polishing sapphire, SiC, etc.

[0002] Polishing pads are used for lapping and polishing optical materials, semiconductor devices, glass substrates for hard disks, sapphire, and SiC. Various types of polishing pads are known, including polishing pads using nonwoven fabric, polishing pads using foamed or non-foamed polyurethane, polishing pads with fixed abrasive grains, and polishing pads using a resin layer with a concave-convex pattern as the polishing surface.

[0003] Among these, the polishing pad using a resin layer having a concave-convex pattern as the polishing surface has the advantage that the grooves forming the concave-convex pattern affect the fluidity of the slurry, and as a result, the object to be polished can be polished uniformly. The manufacturing method of such a polishing pad includes a method of cutting the surface of a flat base material to form grooves, a method of forming a concave-convex pattern on a substrate by applying a screen printing method, and a method of making a mold having a concave-convex pattern and using the mold to mold.

[0004] For example, Patent Document 1 discloses a polishing pad on which a concave-convex pattern is formed by transferring it from a plate having a concave-convex pattern made of photosensitive resin, and Patent Document 2 discloses a polishing pad on which a concave-convex pattern is formed using a mold made of silicone rubber or the like onto which a plate having a concave-convex pattern made of photosensitive resin is transferred. However, the methods of transferring a concave-convex pattern to a resin using an intaglio plate as in Patent Documents 1 and 2 have the problem that the cured resin is difficult to peel off from the intaglio plate, and the convex portions of the resin fall off. In addition, the photosensitive resin and silicone rubber used as the intaglio plate are expensive and have poor durability when used repeatedly, making them unsuitable for mass production.

[0005] JP 2019-178248 JP 2019-178258

[0006] The present invention has been made in consideration of the above problems, and provides a method for manufacturing a polishing pad that is inexpensive and allows the resin to be easily peeled off when a concave-convex pattern is transferred to the resin using an intaglio printing plate.

[0007] As a result of extensive research, the present inventors have discovered a method for manufacturing a polishing pad that can be manufactured inexpensively by using a general-purpose plastic as a disposable intaglio plate, and that can be easily peeled from the resin that forms the polishing layer by using a polyolefin or polystyrene with low surface free energy. The present invention encompasses the following: [1] A method for manufacturing a polishing pad having a polishing layer formed by curing a resin, comprising the steps of: preparing a plastic intaglio plate having a concave-convex pattern formed thereon by vacuum forming or injection molding; pouring the resin raw material into the plastic intaglio plate; curing the resin; and peeling the cured resin from the plastic intaglio plate to obtain the polishing layer. [2] A method for manufacturing a polishing pad as described in [1], wherein the temperature of the plastic intaglio plate is 130°C or less in the resin curing step. [3] A method for manufacturing a polishing pad as described in [1], wherein the plastic intaglio plate is made of a resin selected from polyethylene, polypropylene, polystyrene, and polyvinyl chloride. [4] A method for manufacturing a polishing pad as described in [1], further comprising the step of applying a release agent to the plastic intaglio plate, the release agent being a silicone-based release agent or a fluorine-based release agent. [5] A method for producing a polishing pad according to claim 1, wherein the resin is a thermosetting resin composition. [6] A method for producing a polishing pad according to [1], wherein the resin is a UV-curable resin composition. [7] A method for producing a polishing pad having a polishing layer formed by curing a resin and not containing abrasive grains, comprising the steps of: preparing a plastic intaglio plate having a concave-convex pattern formed by vacuum molding or injection molding; pouring the resin raw material not containing abrasive grains into the plastic intaglio plate; curing the resin; and peeling the cured resin from the plastic intaglio plate to obtain the polishing layer. [8] A method for polishing an object to be polished using a polishing pad obtained by the method for producing a polishing pad according to [7], wherein polishing is performed by free abrasive polishing.[9] A method for manufacturing a polishing pad having a polishing layer formed by curing a resin and containing abrasive grains, comprising the steps of: preparing a plastic intaglio plate having a concave-convex pattern formed by vacuum forming or injection molding; pouring the resin raw material containing abrasive grains into the plastic intaglio plate; curing the resin; and peeling the cured resin from the plastic intaglio plate to obtain the polishing layer.

[10] A method for polishing an object to be polished using a polishing pad obtained by the method for manufacturing a polishing pad described in [9], wherein polishing is performed by fixed abrasive polishing.

[0008] Using general-purpose plastic as a disposable intaglio plate allows for inexpensive production, and using polyolefins or polystyrene, which have low surface free energy, makes it easy to peel off the resin that forms the polishing layer.

[0009] Fig. 1 is a process diagram of a method for producing a polishing layer 11 of a polishing pad of the present invention. Fig. 2 is a cross-sectional view of another embodiment of the polishing layer 11 of a polishing pad of the present invention.

[0010] The following describes in detail an embodiment of the present invention (hereinafter referred to as "the present embodiment"); however, the present invention is not limited to this embodiment, and various modifications are possible without departing from the spirit of the present invention.

[0011] <<Method for Manufacturing a Polishing Pad>> A first embodiment of the method for manufacturing a polishing pad of the present invention will be described using the flowchart of FIG. 1 . The first embodiment is as follows. The polishing pad includes a polishing layer, and the polishing layer includes a polishing surface for polishing an object to be polished. The method for manufacturing a polishing pad having a polishing layer 11 formed by curing a resin 50 includes the steps of: preparing a plastic intaglio 72 having a concave-convex pattern formed thereon by vacuum molding or injection molding (Step 1); applying a mold release agent 8 to the plastic intaglio 72 (Step 2); pouring the resin raw material 50 into the plastic intaglio 72 (Step 3); curing the resin 50 (Step 4); and peeling the cured resin 50 from the plastic intaglio 72 to obtain the polishing layer 11 (Step 5). For convenience, the resin raw material before being poured into a mold (i.e., the resin before curing) and the cured resin will both be referred to as 50 in this specification.

[0012] (Step 1) First, a mold for forming the concave-convex pattern is prepared. There are no particular limitations on the mold, as long as it can form a concave-convex pattern in a plastic material by vacuum forming or injection molding, and examples of the mold include a wooden mold, a resin mold, and a metal mold. Because the plastic intaglio plate 72 on which the concave-convex pattern is formed does not require extremely high durability, a mold that can be repeatedly manufactured is preferred.

[0013] Next, a plastic material for the plastic intaglio 72 is prepared. The plastic material is not particularly limited as long as it is inexpensive and has low surface free energy, but examples include polyolefin resins (polyethylene, polypropylene), polystyrene, and polyvinyl chloride. The surface free energy of the material used for the intaglio 72 of the present invention is preferably 50 mN / m or less, and more preferably 40 mN / m or less. A surface free energy of 50 mN / m or less facilitates the peeling of the polishing layer 11 from the intaglio 72, thereby preventing the protrusions 51 from falling off or being damaged during the peeling of the intaglio 72 and the polishing layer 11. The surface free energy can be calculated by measuring the contact angles with water and methylene iodide using a contact angle meter. Polypropylene (surface free energy: 29.8 mN / m) and polyethylene (surface free energy: 35.6 mN / m) are preferred materials for the intaglio 72 because they are readily available, inexpensive, and have low surface free energy. Examples of polypropylene that can be used include "Elon" manufactured by OJK Corporation and "Hyperl" manufactured by Sanvic, and examples of polyethylene that can be used include "EL-N-AN" manufactured by Resonac.

[0014] The shape of the plastic material is not particularly limited as long as it can be used to produce a plastic intaglio plate 72 with a concave-convex pattern by vacuum forming or injection molding, but a film or sheet is preferred because it is easy to mold. The thickness of the film or sheet-like plastic material is not particularly limited as long as it can be used to produce a plastic intaglio plate 72 with a concave-convex pattern by vacuum forming or injection molding, but a thickness of 0.1 mm to 5 mm is preferred to maintain the strength of the plate and facilitate molding. In the case of vacuum forming, the film or sheet-like plastic material is heated and softened, placed in a mold with a concave-convex pattern, and the space between the plastic material and the mold is evacuated, thereby adhering the plastic material to the mold. Once molding is complete, the plastic material is cooled and removed from the mold to obtain a plastic intaglio plate 72 with a concave-convex pattern. Vacuum forming conditions vary depending on the plastic material, its thickness, etc. In the case of injection molding, the heated and melted plastic material is injected into a mold with a concave-convex pattern, cooled and solidified, and then removed from the mold to obtain a plastic intaglio plate 72 with a concave-convex pattern. The conditions for injection molding vary depending on the plastic material, the thickness of the plastic material intaglio 72, etc. The strength of the plastic intaglio 72 on which the concave-convex pattern has been formed by vacuum molding or injection molding is not particularly limited as long as the concave-convex pattern can be accurately transferred from the plastic intaglio 72 in Step 4 to obtain the polishing layer 11 on which the concave-convex pattern has been formed, but in order to prevent cracking or breaking due to impact, an impact strength of 0.5 J / m or more at 0°C in a DuPont impact test is preferred.

[0015] (Step 2) Next, a release agent 8 is applied to the obtained plastic intaglio 72. The release agent 8 facilitates the separation of the cured resin from the plastic intaglio. There are no particular limitations on the type of release agent, and examples include silicone-based release agents and fluorine-based release agents, with fluorine-based release agents being preferred. There are no particular limitations on the method of applying the release agent 8, as long as it allows the cured resin to be separated from the plastic intaglio, and examples include spraying and electrostatic application, with spraying being preferred.

[0016] (Step 3) The resin raw material 50 is poured into the plastic intaglio 72 coated with the release agent 8. In the present invention, the resin raw material 50 may or may not contain abrasive grains. The polishing pad 1 having an abrasive layer containing abrasive grains is a polishing pad for use in fixed-abrasive polishing. Preferably, the resin raw material 50 is prepared by mixing abrasive grains with a liquid resin before pouring the resin raw material 50 into the plastic intaglio 72. The amount of abrasive grains relative to the resin is not particularly limited, and a conventional content ratio may be used. For example, the abrasive grains may be contained in a ratio of 1% by mass or more to 20% by mass or less, preferably 5% by mass or more to 10% by mass or less, relative to the total resin raw material 50. The type of abrasive grains is not particularly limited, and examples include diamond, cerium oxide, silicon carbide, silicon oxide, zirconium oxide, iron oxide, manganese oxide, magnesium oxide, zinc oxide, titanium oxide, aluminum oxide, zirconium silicate, boron nitride, silicon nitride, barium sulfate, and calcium carbonate. The particle size of the abrasive grains is preferably 1 to 100 μm. On the other hand, the polishing pad 1 having an abrasive layer that does not contain abrasive grains is a polishing pad for use in a free abrasive polishing method, and it is preferable to prepare the resin raw material 50 without mixing abrasive grains into the liquid resin before pouring the resin raw material 50 into the plastic intaglio 72. Even if the polishing pad is for use in a free abrasive polishing method, the abrasive layer used in the polishing pad for the free abrasive polishing method may contain additives other than abrasive grains, but it is preferable not to add additives that affect polishing. The method for pouring the resin raw material 50 into the plastic intaglio 72 is not particularly limited as long as the resin raw material 50 is filled (poured) into the recesses of the plastic intaglio 72. Examples include gravity casting, in which the resin raw material is poured into the recesses under its own weight at room temperature and normal pressure, and vacuum casting, in which the plastic intaglio 72 and the resin 50 are placed in a vacuum container, the pressure is reduced, and the resin is poured into the recesses at atmospheric pressure.

[0017] The resin 50 is not particularly limited as long as a polishing pad using the resin layer 11 having a concavo-convex pattern as the polishing surface can be obtained, but a curable resin composition is preferred. The curable resin composition is not particularly limited, but examples thereof include thermosetting resins; UV-curable resins; photocurable resin compositions containing a photopolymerization initiator and a polymerizable compound; thermosetting resin compositions containing a thermal polymerization initiator and a polymerizable compound; and curable resin compositions containing a two-component mixed curable resin. Furthermore, the curable resin composition may optionally contain a crosslinking agent having two or more polymerizable functional groups.

[0018] The thermosetting resin is not particularly limited, but examples thereof include phenol resin, epoxy resin, acrylic resin, urethane resin, and formaldehyde resin.

[0019] The UV-curable resin is not particularly limited, but for example, a prepolymer having a number-average molecular weight of about 1,000 to 10,000 is preferable, and examples of the material include isocyanurate-based resins, acrylic (methacrylic) ester resins and urethane-modified resins thereof, and thiokol-based resins, and a reactive diluent or organic solvent can be used as appropriate depending on the application.

[0020] Examples of photopolymerization initiators include benzophenone compounds, acetophenone compounds, and thioxanthone compounds. Examples of thermal polymerization initiators include azo compounds such as 2,2'-azobisbutyronitrile, and peroxides such as methyl ethyl ketone peroxide and benzoyl peroxide (BPO).

[0021] Specific examples of the resin include unsaturated carboxylic acids having a polymerizable unsaturated group, such as (meth)acrylic acid, itaconic acid, crotonic acid, isocrotonic acid, and maleic acid; unsaturated carboxylic acid esters having a polymerizable unsaturated group, such as (meth)acrylate, epoxy (meth)acrylate (vinyl ester resin), urethane (meth)acrylate, and polyester (meth)acrylate; polyesters having an unsaturated group; polyethers having a polymerizable unsaturated group; polyamides having a polymerizable unsaturated group; urethanes having a polymerizable unsaturated group; aromatic compounds having a polymerizable unsaturated group, such as styrene, and vinyl ester resins.

[0022] The two-component mixed curable resin is not particularly limited, but examples thereof include prepolymers with different physical properties, such as epoxy resin, unsaturated polyester resin, and polyamide resin.

[0023] Among these, those that cure at room temperature are preferred in terms of the heat resistance of the plastic intaglio 72. Examples include curable resin compositions containing a polymerization initiator that works at room temperature, UV-curable resins and photocurable resin compositions that cure upon exposure to light, and mixed curable resin compositions that cure by mixing two liquids. Furthermore, in terms of polishing (lapping) performance, vinyl ester resins or unsaturated polyester resins, which have high heat resistance (high deformation temperature), are preferred.

[0024] A step of embedding a sheet-like fiber material 6 in the resin 50 before the resin 50 hardens may be further included. By embedding the fiber material 6 inside the resin 50, the strength of the convex portions 51 is increased, and a polishing layer 11 is obtained that can prevent the polishing pad convex portions 51 from falling off during manufacturing (when peeling from the plastic intaglio 72) and during polishing.

[0025] Furthermore, the method may further include a step of bonding a substrate to the surface of the resin 50 opposite to the surface that contacts the plastic intaglio 72 before curing the resin 50. By using a substrate, the resin 50 is cured in a state where it is sandwiched between the substrate and the plastic intaglio 72. This tends to improve the uniformity of the thickness of the obtained cured product and further improve the flatness of the back surface of the obtained cured product (the surface opposite to the surface that contacts the plastic intaglio 72).

[0026] (Step 4) The process of curing the resin raw material 50 will be described. The method for curing the resin raw material 50 is not particularly limited as long as it is suitable for each resin raw material 50. Depending on the properties of the resin, examples include a photocuring method using ultraviolet light or the like, a thermal curing method using heat (including a method of leaving the material at room temperature), or a method of mixing and leaving the material in a two-component mixture. The light to be irradiated is not particularly limited as long as it can cure the resin raw material 50, but examples include ultraviolet light. Examples of light sources that emit such light include high-pressure mercury lamps, UV-LED lamps, and black light fluorescent lamps (BLBs), with BLBs being preferred. The light irradiation direction may be from either the lower surface 72A of the plastic intaglio 72 or the upper surface 50A of the resin raw material 50. In particular, when using a plastic intaglio 72, its transparency allows sufficient light to pass through to cure the convex portions 51, even when irradiated from the lower surface 72A, ensuring sufficient curing of the convex portions 51. This was not possible with conventional molding dies made of silicone rubber, etc. The wavelength of the ultraviolet light irradiation is preferably 200 nm to 400 nm, and the irradiation time is preferably 3 minutes to 30 minutes.

[0027] (Step 5) The cured resin 50 is peeled off from the plastic intaglio 72 to obtain the polishing layer 11. The peeling method is not particularly limited, and may include holding the edge of the cured resin and peeling it off from the intaglio 72. The resulting polishing layer 11 has a concave-convex pattern transferred from the plastic intaglio 72, and the surface of the convex portions 51 of the concave-convex pattern serves as the polishing surface for polishing the workpiece. Alternatively, the plastic intaglio 72 may be peeled off from the cured resin 50. Since the plastic intaglio 72 used in the polishing pad manufacturing method of the present invention is disposable, deformation or damage may occur when peeling the plastic intaglio 72 from the cured resin 50. This prevents damage or deformation of the polishing layer 11, and prevents the convex portions 51 of the resin 50 from falling off. The peeled polishing layer 11 can be cut to a predetermined size so that it can be used in a polishing pad. If necessary, a cushioning layer can be attached to the surface opposite the concave-convex pattern to form a polishing pad.

[0028] The resulting abrasive layer 11 has a bending strength of 30 MPa or more, preferably 30 to 1000 MPa, more preferably 40 to 900 MPa, and even more preferably 50 to 800 MPa. The bending strength is obtained by measurement performed in accordance with JIS K7203. When the bending strength is within the above range, breakage or deformation of the abrasive layer 11 can be suppressed when the abrasive layer 11 is peeled off from the plastic intaglio 72.

[0029] FIG. 2 shows an enlarged view of a polishing layer 11 having a different shape from that shown in FIG. 1 . The polishing layer 11 differs from the polishing layer 11 of FIG. 1 in that it includes a recess 53 on the opposite side of the protrusion 51. By including the recess 53, further weight reduction and cost reduction can be achieved. The recess 53 can be formed by intentionally reducing the amount of resin in the area where the protrusion 51 is to be formed in Step 3, or by pressing a mold corresponding to the recess 53 from above after Step 3. The shape of the recess 53 is not particularly limited, and may be a shape with corners (e.g., a truncated quadrangular pyramid) as shown in FIG. 2 or a shape with curved surfaces (e.g., a dome shape).

[0030] (Polishing Method) The polishing method using the polishing pad 1 obtained by the manufacturing method of the present invention is preferably used in free abrasive polishing. Here, free abrasive polishing is a method of polishing using a slurry mixed with a liquid without fixed abrasive grains. That is, it is a method of polishing using a slurry containing abrasive grains (abrasive grain-containing solution). Therefore, the polishing layer of the polishing pad 1 does not contain abrasive grains. Compared to fixed abrasive grains, there are fewer problems such as scratch generation. In particular, when scratch generation is minimized, for example, when performing final finishing, by using the polishing pad 1 obtained by the manufacturing method of the present invention, it is possible to minimize scratch generation on the polished object at a low cost.

[0031] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0032] In each example and comparative example, unless otherwise specified, "parts" means "parts by mass."

[0033] (Manufacturing of polishing pads)

[0034] (Manufacture of Polishing Pad 1) A polypropylene resin sheet was vacuum-formed to produce a plastic intaglio 72 having multiple truncated pyramidal recesses with a height of 0.85 mm and bases of 1.5 mm square. Next, 90 parts of unsaturated polyester resin (product name: Rigolac, manufactured by Resonac Co., Ltd.) was poured into the plastic intaglio 72. Before curing, a polypropylene mesh fabric with a fiber diameter of 150 μm, a mesh size of 30 μm, and a thickness of 300 μm was sunk into the resin 50 from above, allowing the fiber material to penetrate into the base 52. After curing the resin 50 at room temperature (25°C) for 30 minutes, the resin 50 was peeled off from the plastic intaglio 72, thereby producing the polishing pad 1.

[0035] (Manufacture of Polishing Pad 2) Polishing pad 2 was manufactured in the same manner as polishing pad 1, except that the polishing pad material was made of vinyl ester resin (product name: Lipoxy, manufactured by Resonac Co., Ltd.) instead of unsaturated polyester resin, and the mesh fabric material was made of polyethylene fiber instead of polypropylene fiber.

[0036] (Manufacture of Polishing Pad 3) Polishing Pad 3 was manufactured in the same manner as Polishing Pad 1, except that a UV-curable resin (product name: SR368D NS (tris(2-hydroxyethyl)isocyanurate acrylate), manufactured by Arkema) containing 12 mass% of abrasive grains (product name: SQDP, manufactured by Surface, particle size 4 μm) was used instead of the unsaturated polyester resin, and the resin was cured by irradiating with ultraviolet light without incorporating any fibrous material.

[0037] Furthermore, in manufacturing polishing pads 2 and 3, it was confirmed that even if the material of the polishing pad, the material of the mesh fabric, the presence or absence of abrasive grains, etc. were changed, polishing pads similar to polishing pad 1 could also be manufactured using a plastic intaglio plate made of polypropylene resin.

[0038] Furthermore, a polishing pad 1 without a mesh fabric was also manufactured using the same manufacturing method (polishing pad 4), and a polishing pad 2 without a mesh fabric was also manufactured using the same manufacturing method (polishing pad 5).

[0039] (When peeling from the intaglio) A peeling roller was used to conduct a peeling experiment on the resin 50 from the plastic intaglio 72. Examples of the peeling roller include a combination of adhesive tape and a rod-shaped peeling roller, as described in JP-A-9-114384. Peeling experiments were conducted under conditions that allowed the intaglio and resin 50 to be peeled off using the plastic intaglio 72 of the above example and using silicone rubber instead of plastic as the intaglio. The results showed that the silicone rubber intaglio required a large force to peel, and that the convex portions 51 of the peeled resin 50 were damaged or lost. In contrast, the polishing pads 1 to 5 obtained using the plastic intaglio 72 made of polypropylene resin did not suffer from any damage or loss of the convex portions 51 during peeling.

[0040] The method for manufacturing a polishing pad of the present invention is an inexpensive method for manufacturing a polishing pad that facilitates resin peeling from an intaglio plate, and therefore has industrial applicability as a method for manufacturing polishing pads used for lapping and polishing optical materials, semiconductor devices, glass substrates for hard disks, etc.

[0041] REFERENCE SIGNS LIST 11 Polishing layer 50 Resin raw material 50A Upper surface of resin raw material 51 Convex portion 52 Base portion 53 Concave portion 71 Plastic material 72 Plastic intaglio 72A Lower surface of plastic intaglio 8 Mold release agent

Claims

1. A method for manufacturing a polishing pad having a polishing layer formed by hardening a resin, comprising the steps of: preparing a plastic intaglio plate on which a concave-convex pattern is formed by vacuum forming or injection molding; pouring the resin raw material into the plastic intaglio plate; hardening the resin; and peeling the hardened resin from the plastic intaglio plate to obtain the polishing layer.

2. The method for producing a polishing pad according to claim 1, wherein the temperature of the plastic intaglio is 130° C. or less in the step of curing the resin.

3. The method for producing a polishing pad according to claim 1, wherein the plastic intaglio is made of a resin selected from the group consisting of polyethylene, polypropylene, polystyrene, and polyvinyl chloride.

4. The method for producing a polishing pad according to claim 1, further comprising a step of applying a release agent to said plastic intaglio plate, said release agent being a silicone-based release agent or a fluorine-based release agent.

5. The method for producing a polishing pad according to claim 1, wherein the resin is a thermosetting resin composition.

6. The method for producing a polishing pad according to claim 1, wherein the resin is a UV-curable resin composition.

7. A method for manufacturing a polishing pad having an abrasive layer formed by hardening a resin and not containing abrasive grains, comprising the steps of: preparing a plastic intaglio plate having a concave-convex pattern formed by vacuum molding or injection molding; pouring the resin raw material not containing abrasive grains into the plastic intaglio plate; hardening the resin; and peeling the hardened resin from the plastic intaglio plate to obtain the abrasive layer.

8. A method for polishing an object to be polished using a polishing pad obtained by the method for producing a polishing pad according to claim 7, comprising the step of performing the polishing by free abrasive polishing.

9. A method for manufacturing a polishing pad having an abrasive layer formed by hardening a resin and containing abrasive grains, comprising the steps of: preparing a plastic intaglio plate having a concave-convex pattern formed by vacuum molding or injection molding; pouring the resin raw material containing abrasive grains into the plastic intaglio plate; hardening the resin; and peeling the hardened resin from the plastic intaglio plate to obtain the abrasive layer.

10. A method for polishing an object to be polished using a polishing pad obtained by the method for producing a polishing pad according to claim 9, comprising the step of carrying out the polishing by fixed abrasive polishing.

Citation Information

Patent Citations

  • Composite stamper

    JP2000135718A

  • Polishing pad and its manufacturing method

    JP2005074614A

  • Stamper made of resin and micropart manufactured using the same

    JP2006346905A

  • Stamper for injection mold

    JP2006347087A

  • Transfer mold

    JP2007521985A