Lithium secondary battery
The pouch-type lithium secondary battery design with a sintered lithium composite oxide positive electrode and carbon-based negative electrode, combined with a specific electrolyte composition, effectively addresses the challenge of maintaining performance in high-temperature and reduced-pressure environments by minimizing dimensional changes and ensuring high discharge capacity retention.
Patent Information
- Application Number
- PCT/JP2024/011273
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-03
AI Technical Summary
Lithium secondary batteries face challenges in maintaining good characteristics, such as discharge capacity, in high-temperature and reduced-pressure environments, where they often experience significant dimensional changes and performance degradation.
A pouch-type lithium secondary battery design featuring a sintered lithium composite oxide positive electrode, a carbon-based negative electrode, and a specific electrolyte composition with a mixed solvent system, including esters and lactones, which helps maintain a stable thickness ratio and suppresses swelling, ensuring consistent performance under extreme conditions.
The battery maintains good characteristics and discharge capacity retention rates of 70% or more even at 80°C and 100 Pa, preventing significant dimensional changes and performance degradation, thus ensuring reliable operation in high-temperature and reduced-pressure environments.
Smart Images

Figure JP2024011273_03102024_PF_FP_ABST
Abstract
Description
Lithium secondary battery
[0001] The present disclosure relates to a lithium secondary battery. This application claims priority to Japanese Application No. 2023-056460, filed on March 30, 2023, and incorporates by reference all of the contents of said Japanese application.
[0002] A technology related to a pouch-type lithium secondary battery is disclosed, for example, in Japanese Patent Laid-Open Publication No. 2017-79192 (Patent Document 1). Conventionally, a powder-dispersed positive electrode active material formed by molding a mixture of a lithium composite oxide (i.e., lithium transition metal oxide) powder, a binder, a conductive agent, etc., has been known as a positive electrode active material for lithium secondary batteries (also called lithium ion secondary batteries). Meanwhile, Japanese Patent No. 5587052 (Patent Document 2) proposes a technology for increasing the capacity of a positive electrode by using a lithium composite oxide sintered plate as the positive electrode active material bonded to a positive electrode current collector. Furthermore, Japanese Patent No. 6943970 (Patent Document 3) proposes a heat-resistant lithium secondary battery that does not expand even at high temperatures of 150°C, by using a negative electrode containing carbon and styrene-butadiene rubber (SBR) in addition to a lithium composite oxide sintered plate, and an electrolyte solution containing lithium fluoroborate (LiBF4) in a non-aqueous solvent made of γ-butyrolactone (GBL) or γ-butyrolactone (GBL) and ethylene carbonate (EC).
[0003] JP 2017-79192 A, Patent No. 5587052, Patent No. 6943970
[0004] Recently, lithium secondary batteries are sometimes used in high-temperature and low-pressure environments, and even in such environments, they are required to maintain good characteristics, such as not significantly reducing discharge capacity compared to normal temperature and pressure environments.
[0005] Therefore, one of the objects is to provide a lithium secondary battery that can maintain good characteristics even in a high-temperature environment and a reduced-pressure environment.
[0006] The lithium secondary battery according to the present disclosure is a pouch-type lithium secondary battery. The lithium secondary battery includes: a positive electrode layer made of a sintered lithium composite oxide; a negative electrode layer; a separator interposed between the positive electrode layer and the negative electrode layer; an electrolytic solution containing an electrolyte and a solvent impregnated in the positive electrode layer, the negative electrode layer, and the separator; and an exterior body having a sealed space and accommodating the positive electrode layer, the negative electrode layer, the separator, and the electrolytic solution. In the thickness direction of the positive electrode layer, the ratio of the thickness of the exterior body at a temperature of 80°C and a pressure of 100 Pa to the thickness of the exterior body at a temperature of 25°C and a pressure of 101,325 Pa is 1.05 to 2.63.
[0007] Such a lithium secondary battery can maintain good characteristics even in a high-temperature environment and a reduced-pressure environment.
[0008] Fig. 1 is a schematic plan view showing the structure of a lithium secondary battery according to the present disclosure. Fig. 2 is a schematic cross-sectional view showing the structure of a lithium secondary battery according to the present disclosure. Fig. 3 is a schematic view showing a cross-section of a lithium secondary battery according to the present disclosure. Fig. 4 is a schematic view showing an assembly process of a lithium secondary battery. Fig. 5 is a schematic cross-sectional view showing a part of a measuring device used when measuring the thickness of an exterior body.
[0009] [Summary of the Embodiments] First, embodiments of the present disclosure will be described. The lithium secondary battery according to the present disclosure is a pouch-type lithium secondary battery. The lithium secondary battery includes a positive electrode layer made of a sintered lithium composite oxide, a negative electrode layer, a separator interposed between the positive electrode layer and the negative electrode layer, an electrolyte solution containing an electrolyte and a solvent impregnated into the positive electrode layer, the negative electrode layer, and the separator, and an exterior body having a sealed space in which the positive electrode layer, the negative electrode layer, the separator, and the electrolyte solution are accommodated. In the thickness direction of the positive electrode layer, the ratio of the thickness of the exterior body at a temperature of 80°C and a pressure of 100 Pa to the thickness of the exterior body at a temperature of 25°C and a pressure of 101,325 Pa is 1.05 or more and 2.63 or less.
[0010] The lithium secondary battery having such a configuration exhibits relatively small changes in thickness even under high-temperature and reduced-pressure environments, which prevents the distance between the positive electrode layer and the negative electrode layer from increasing in the thickness direction. As a result, the battery can maintain good characteristics even under high-temperature and reduced-pressure environments.
[0011] In the lithium secondary battery of the above embodiment, the positive electrode layer may be a plate-shaped electrode. The negative electrode layer may be a plate-shaped electrode. By doing so, it is possible to relatively reduce the dimensional change in the thickness direction due to expansion or the like in both the positive electrode layer and the negative electrode layer, even in a high-temperature environment and a reduced-pressure environment. Therefore, it is possible to maintain better characteristics even in a high-temperature environment and a reduced-pressure environment.
[0012] In any one of the above lithium secondary batteries, the solvent may be a mixed liquid solvent containing a first substance that is an ester and has a carbonate group and a second substance that is an ester different from the first substance and has a carbonate or lactone group. The volume ratio of the first substance to the second substance may be within a range of 1:10 or more and 10:1 or less. An electrolyte solution using such a solvent has a relatively low vapor pressure and is less likely to produce reaction products due to side reactions. This configuration makes it difficult for the exterior body to swell, thereby further suppressing the increase in the distance between the positive electrode layer and the negative electrode layer. Therefore, better characteristics can be maintained even in high-temperature and reduced-pressure environments. If the volume ratio is outside this range, it is difficult to achieve the effect of lowering the vapor pressure sufficiently to suppress the exterior body from swell in high-temperature and reduced-pressure environments. Alternatively, battery characteristics may be degraded due to increased electrolyte viscosity or difficulty in forming an SEI (Solid Electrolyte Interface) coating on the electrode surface.
[0013] In any one of the above lithium secondary batteries, the electrolyte concentration may be 2.0 mol / L or more and 8.0 mol / L or less. By doing so, a relatively high electrolyte concentration results in a relatively low vapor pressure, and the generation of reaction products due to side reactions is reduced. This configuration makes it difficult for the exterior body to expand, further suppressing the distance between the positive electrode layer and the negative electrode layer from increasing. Therefore, good characteristics can be maintained even in high-temperature and reduced-pressure environments.
[0014] The lithium secondary battery of any one of the above aspects may further include an adhesive made of a mixed resin of an acid-modified polyolefin resin and an epoxy resin, the adhesive bonding at least one of the positive electrode layer or the negative electrode layer to the exterior body in an enclosed space. By using such an adhesive to bond the positive electrode layer or the negative electrode layer to the exterior body, it is possible to suppress wrinkling of the exterior body when the lithium secondary battery of the present disclosure is used as a power supply source in a sheet-like device or a flexible device.
[0015] The lithium secondary battery according to any one of the above aspects may further include an adhesive composed of a mixed resin of an acid-modified polyolefin resin and an epoxy resin, the adhesive bonding at least one of the positive electrode layer or the negative electrode layer to the exterior body in a sealed space. The positive electrode layer may be a plate-shaped electrode. The negative electrode layer may be a plate-shaped electrode or a coated electrode. The solvent may be a mixed solvent containing sulfolane and γ-butyrolactone. The volume ratio of sulfolane to γ-butyrolactone may be 7:3 or more and 4:1 or less. The electrolyte concentration may be 1.5 mol / L or more and 5.0 mol / L or less. A lithium secondary battery having such a configuration can reliably maintain better characteristics even in high-temperature and reduced-pressure environments.
[0016] [Specific Example of Embodiment] Next, specific examples of the lithium secondary battery of the present disclosure will be described with reference to the drawings. In the following drawings, the same or corresponding parts are designated by the same reference characters, and description thereof will not be repeated.
[0017] (Embodiment) A lithium secondary battery according to the present disclosure will be described. FIG. 1 is a schematic plan view showing the structure of a lithium secondary battery according to the present disclosure (hereinafter, sometimes simply referred to as a "battery"). FIG. 2 is a schematic cross-sectional view showing the structure of a lithium secondary battery according to the present disclosure. FIG. 3 is a diagram showing a schematic cross-section of a lithium secondary battery according to the present disclosure. Note that in FIGS. 1, 2, and 3, some components are enlarged, emphasized, or omitted to facilitate understanding. Furthermore, the components shown in FIGS. 1, 2, and 3 do not necessarily reflect actual dimensional relationships.
[0018] 1, 2, and 3, a battery 11, which is a lithium secondary battery according to the present disclosure, is pouch-shaped. The battery 11 according to the present disclosure is effectively used in high-temperature and reduced-pressure environments, such as a power source for a temperature sensor that detects the temperature of a chamber in a semiconductor manufacturing device. A high-temperature environment refers to a temperature of 80°C or higher, and a reduced-pressure environment refers to a pressure of 100 Pa (Pascal) or lower.
[0019] The battery 11 includes a pair of exterior films 13, 14 that constitute an exterior body 12, a positive electrode tab terminal 15, and a negative electrode tab terminal 16. The exterior films 13, 14 have the same rectangular shape in a plan view (i.e., the state shown in FIG. 1 ). The four peripheral edges of the exterior films 13, 14 are joined to each other except for portions that face each other across the positive electrode tab terminal 15 and the negative electrode tab terminal 16. The specific manner of joining is not particularly limited, and the films can be joined by, for example, adhesion, fusion, or the like.
[0020] The battery 11 is a small, thin battery. The dimensions of the battery 11 (external dimensions of the exterior body 12) are not particularly limited, but may be, for example, a vertical length of 10 mm (millimeters) to 46 mm (10 mm or more and 46 mm or less) and a horizontal length of 10 mm to 46 mm. The thickness of the battery 11 (external thickness of the exterior body 12) may be, for example, 0.3 mm to 0.45 mm, preferably 0.4 mm (400 μm (micrometers)) to 0.45 mm. The battery 11 is, as a whole, a sheet-like or flexible plate-like article.
[0021] In the battery 11, a sealed space 17 is formed between the opposing inner surfaces of the exterior films 13 and 14. The sealed space 17 houses a battery body. The battery 11 includes a positive electrode 21, a negative electrode 22, a separator 23, and an electrolyte 24. In the battery 11, the positive electrode 21, the negative electrode 22, the separator 23, and the electrolyte 24 are sometimes collectively referred to as the battery body. The positive electrode 21, the negative electrode 22, and the separator 23 are stacked in a predetermined stacking direction. In the example shown in FIG. 2, the positive electrode 21, the separator 23, and the negative electrode 22 are stacked in the vertical direction in FIG. 2. That is, the positive electrode 21 and the negative electrode 22 face each other with the separator 23 interposed therebetween. In the following description, the upper and lower sides in FIG. 2 are referred to as the "upper side" and "lower side" of the battery 11, respectively. The vertical direction in FIG. 2 is also referred to as the "vertical direction" or the "stacking direction."
[0022] The exterior body 12 is a bag formed by joining the peripheries of exterior films 13 and 14. The exterior films 13 and 14 are each formed from a laminate sheet in which metal foils 25 and 26 made of a metal such as aluminum (Al) are stacked with insulating resin layers 27 and 28. The exterior films 13 and 14 are arranged so that the metal foils 25 and 26 are located on the outside of the bag body and the resin layers 27 and 28 are located on the inside of the bag body. The thickness of the exterior body 12 is shown as thickness T in FIG. 3.
[0023] The exterior body 12 covers the entire battery body. The exterior body 12 is a bag-like body that houses the positive electrode 21, the negative electrode 22, the separator 23, and the electrolyte 24. The electrolyte 24 is present continuously around the positive electrode 21, the separator 23, and the negative electrode 22. In other words, the electrolyte 24 is interposed between the positive electrode 21 and the negative electrode 22. The electrolyte 24 is impregnated into the positive electrode 21, the separator 23, and the negative electrode 22. The positive electrode tab terminal 15 and the negative electrode tab terminal 16 extend to the outside of the exterior body 12. Inside the exterior body 12, the positive electrode tab terminal 15 is connected to the positive electrode current collector 31. With this configuration, the positive electrode tab terminal 15 is electrically connected to the positive electrode 21. The negative electrode tab terminal 16 is connected to the negative electrode current collector 36. With this configuration, the negative electrode tab terminal 16 is electrically connected to the negative electrode 22.
[0024] The positive electrode tab terminal 15 and the negative electrode tab terminal 16 each have a strip-like shape. The positive electrode tab terminal 15 includes a main body made of a conductive material and a protective layer made of resin arranged to cover the surface of the main body. Like the positive electrode tab terminal 15, the negative electrode tab terminal 16 also includes a main body made of a conductive material and a protective layer made of resin arranged to cover the surface of the main body. Metals such as aluminum (Al) and nickel (Ni) can be used as the conductor that constitutes the main body.
[0025] The separator 23 is disposed on the upper surface of the positive electrode 21 in the stacking direction. The negative electrode 22 is disposed on the upper surface of the separator 23. That is, the negative electrode 22 is disposed in contact with the upper surface side of the separator 23. The positive electrode 21 is disposed in contact with the lower surface side of the separator 23. The positive electrode 21, the negative electrode 22, and the separator 23 each have, for example, a rectangular shape in a plan view. The positive electrode 21 and the negative electrode 22 have approximately the same shape and dimensions in a plan view. The separator 23 may have dimensions larger than the positive electrode 21 and the negative electrode 22, respectively, in order to prevent internal short circuits. The positive electrode 21 and the negative electrode 22 face each other almost entirely, except for misalignment that occurs during the manufacturing process or use.
[0026] The dimensions and shape of the positive electrode 21 in plan view (i.e., the dimensions and shape of the main surface of the positive electrode 21) may be, for example, a rectangle with a side length of 9.75 mm to 28.5 mm. Preferably, the dimensions and shape of the positive electrode 21 in plan view (i.e., the area of the main surface of the positive electrode 21) may be, for example, a rectangle with a side length of 18.15 mm to 25.5 mm. 2 ~812mm 2 Preferably, it is 441 mm 2 ~812mm 2 may be.
[0027] The dimensions, shape, and area of the negative electrode 22 may be similar to those of the positive electrode 21. Alternatively, the dimensions of the negative electrode 22 may be slightly larger (by about 4% to 7%) than those of the positive electrode 21. That is, the dimensions and shape of the negative electrode 22 in plan view (i.e., the dimensions and shape of the main surface of the negative electrode 22) may be, for example, a rectangle with a side length of 10.45 mm to 29.2 mm. Preferably, the dimensions and shape of the negative electrode 22 in plan view (i.e., the area of the main surface of the negative electrode 22) may be, for example, 109 mm 2 ~852mm 2 Preferably, it is 470 mm 2 ~852mm 2 may be.
[0028] (Positive Electrode Structure 1) The positive electrode 21 includes a positive electrode current collector 31, a positive electrode active material plate 32, and a conductive bonding layer 33. The positive electrode current collector 31 is a sheet-like member having electrical conductivity. The positive electrode 21 is a so-called plate-like electrode. The lower surface of the positive electrode current collector 31 is bonded to the resin layer 27 of the exterior body 12 via a positive electrode bonding layer 34. The positive electrode bonding layer 34 is formed, for example, from a mixed resin of an acid-modified polyolefin resin and an epoxy resin. The positive electrode bonding layer 34 may also be formed from other materials. The thickness of the positive electrode bonding layer 34 is, for example, 0.5 μm to 10 μm.
[0029] The positive electrode current collector 31 includes a metal foil made of a metal such as aluminum and a conductive carbon layer laminated on the upper surface of the metal foil. In other words, the main surface of the positive electrode current collector 31 facing the positive electrode active material plate 32 is coated with a conductive carbon layer. The metal foil may be made of various metals other than aluminum (e.g., copper, nickel, silver, gold, chromium, iron, tin, lead, tungsten, molybdenum, titanium, zinc, or alloys containing any of these). Furthermore, the positive electrode current collector 31 does not necessarily need to include a conductive carbon layer.
[0030] The positive electrode active material plate 32 is a thin plate-shaped ceramic sintered body containing a lithium composite oxide. Preferably, the positive electrode active material plate 32 is composed substantially only of the lithium composite oxide. A separator 23 is laminated on the upper surface of the positive electrode active material plate 32. Gold (Au) or the like may be sputtered onto the positive electrode active material plate 32 as a current collection aid.
[0031] The positive electrode active material plate 32 has a structure in which a plurality of (i.e., a large number of) primary particles are bonded together. The primary particles are composed of a lithium composite oxide having a layered rock salt structure. The lithium composite oxide is a composite oxide of lithium and a transition metal element M (general formula: Li p MO 2 (wherein 0.05≦p≦1.10), a portion of p is substituted with a substituting metal element, which is another metal element. The transition metal element M includes, for example, one or more selected from cobalt (Co), nickel (Ni), and manganese (Mn). The transition metal element M is the main metal other than lithium contained in the lithium composite oxide, and will be referred to as the "main transition metal element" hereinafter.
[0032] Examples of composite oxides of lithium and a transition metal element M include lithium cobalt oxide (Li p CoO 2 (wherein 1≦p≦1.1)), lithium nickel oxide (LiNiO 2 ), lithium manganate (Li 2 MnO 3 ), lithium nickel manganese oxide (Li p (Ni 0.5 , Mn 0.5 ) O 2 ), general formula: Li p (Co x , Ni y , Mn z ) O 2 (wherein 0.97≦p≦1.07, x+y+z=1), a solid solution represented by Li p (Co x , Ni y , Al z ) O 2(wherein 0.97≦p≦1.07, x+y+z=1, 0<x≦0.25, 0.6≦y≦0.9, and 0<z≦0.1), or a solid solution represented by the formula: Li 2 MnO 3 and LiMO 2 (wherein M is a transition metal such as Co or Ni) is particularly preferably a solid solution of lithium cobalt oxide, Li p CoO 2 (wherein 1≦p≦1.1), for example, LiCoO 2 is.
[0033] The transition metal element M may be one or more of elements such as magnesium (Mg), aluminum (Al), silicon (Si), calcium (Ca), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu), zinc (Zn), gallium (Ga), germanium (Ge), strontium (Sr), yttrium (Y), zirconia (Zr), niobium (Nb), molybdenum (Mo), silver (Ag), tin (Sn), antimony (Sb), tellurium (Te), barium (Ba), and bismuth (Bi). Titanium (Ti) or niobium (Nb) is preferred.
[0034] The layered rock salt structure is a crystal structure in which lithium layers and transition metal layers other than lithium are alternately stacked with oxygen layers sandwiched between them. That is, the layered rock salt structure is a crystal structure in which metal ion layers other than lithium and lithium layers are alternately stacked with oxide ions interposed between them. Typically, α-NaFeO 2 This is a structure in which transition metals and lithium are regularly arranged in the
[111] axis direction of a cubic rock salt structure.
[0035] The conductive bonding layer 33 includes a conductive powder and a binder. The conductive powder is, for example, a powder of acetylene black, flake natural graphite, carbon nanotubes, carbon nanofibers, carbon nanotube derivatives, or carbon nanofiber derivatives. The binder includes, for example, a polyimide amide resin. The binder may contain one or more types of polyimide amide resin. The binder may also contain a resin other than polyimide amide resin. The conductive bonding layer 33 can be formed by applying a liquid or paste adhesive containing the conductive powder, binder, and a solvent to the positive electrode current collector 31 or the positive electrode active material plate 32, and then evaporating the solvent between the positive electrode current collector 31 and the positive electrode active material plate 32 to solidify the adhesive.
[0036] The thickness of the positive electrode current collector 31 is, for example, 9 μm to 50 μm, preferably 9 μm to 20 μm, and more preferably 9 μm to 15 μm. The thickness of the positive electrode active material plate 32 is, for example, 15 μm to 200 μm, preferably 30 μm to 150 μm, and more preferably 50 μm to 100 μm. The thickness of the conductive bonding layer 33 is, for example, 3 μm to 28 μm, and preferably 5 μm to 25 μm.
[0037] (Positive Electrode Structure 2) In the lithium secondary battery according to the present disclosure, the positive electrode 21 is not limited to a plate-shaped electrode. That is, the positive electrode 21 may be a coated electrode. In this case, the positive electrode 21 includes the above-described positive electrode current collector 31 and a positive electrode active material layer coated on the positive electrode current collector 31. The positive electrode active material layer includes the above-described lithium composite oxide as a positive electrode active material and a binder mainly composed of a resin. As described above, the lithium composite oxide is a composite oxide of lithium and a main transition metal element (e.g., Co, Ni, Mn) in which a portion of the lithium composite oxide is substituted with a substituting metal element (e.g., Nb, Ti). The binder is, for example, styrene butadiene rubber (SBR), polyvinylidene fluoride (PVDF), or a mixture thereof.
[0038] An example of a method for manufacturing the positive electrode 21 when the positive electrode 21 is a coated electrode will be described below. In the following description, the case where the main transition metal element and the substituting metal element are Co and Nb, respectively, will be described. First, a mixed powder of an oxide of lithium and an oxide of a main transition metal element (i.e., Co) is prepared, as in the case where the positive electrode 21 includes the positive electrode active material plate 32. The mixed powder is maintained at 900°C for 10 hours.
[0039] Next, in the same manner as when the positive electrode 21 includes the positive electrode active material plate 32, Nb 2 O 5 Powder (manufactured by Mitsui Mining & Smelting Co., Ltd.) is added to the raw material powder, which is then crushed and pulverized in a pot mill so that the volumetric D50 particle size distribution is 0.8 μm. 2 O 5 The powder addition rate is 0.03 mass%, and the Nb content in the raw material powder is 0.021 mass%. The volume-based D50 particle size of the raw material powder may be changed as appropriate, for example, within a range of 0.2 μm to 10 μm. The Nb content in the raw material powder may also be changed as appropriate, for example, within a range of 0.1 mass% to 2.0 mass%.
[0040] Next, 91% by mass of the raw material powder, 5% by mass of acetylene black, 4% by mass of polyvinylidene fluoride (PVDF), and an N-methylpyrrolidone (NMP) solution are mixed to prepare a slurry. The slurry is then applied to a positive electrode current collector 31 (e.g., an aluminum foil with a thickness of 10 μm) and dried. The dried coating layer is then pressed to produce a positive electrode 21, which is a coated electrode.
[0041] The obtained positive electrode 21 is combined with other components in the same manner as in Example 1 of battery production to obtain a lithium secondary battery 11 .
[0042] (Negative Electrode Structure 1) The negative electrode 22 includes a negative electrode current collector 36 and a negative electrode active material layer 37. The negative electrode current collector 36 is a sheet-like member having electrical conductivity. The upper surface of the negative electrode current collector 36 is bonded to the resin layer 28 of the exterior film 14 via a negative electrode bonding layer 38. The negative electrode active material layer 37 is coated on the lower surface of the negative electrode current collector 36. In other words, the negative electrode 22 is a so-called coated electrode. The negative electrode active material layer 37 faces the separator 23 in the vertical direction.
[0043] The negative electrode bonding layer 38 is formed of, for example, a mixed resin of an acid-modified polyolefin resin and an epoxy resin, but may also be formed of various other materials.
[0044] The negative electrode current collector 36 is, for example, a metal foil made of a metal such as copper. The metal foil may be made of various metals other than copper (for example, copper, stainless steel, nickel, aluminum, silver, gold, chromium, iron, tin, lead, tungsten, molybdenum, titanium, zinc, or alloys containing any of these).
[0045] The negative electrode active material layer 37 includes a binder primarily composed of resin and a carbonaceous material serving as the negative electrode active material. Examples of the carbonaceous material include natural graphite, artificial graphite, pyrolytic carbon, coke, baked resin, mesophase microspheres, and mesophase pitch. In the negative electrode 22, a lithium-storing material may be used as the negative electrode active material instead of the carbonaceous material. Examples of the lithium-storing material include silicon, aluminum, tin, iron, iridium, or alloys, oxides, or fluorides containing these elements. The binder may be, for example, styrene butadiene rubber (SBR), polyvinylidene fluoride (PVDF), or a mixture thereof.
[0046] The thickness of the negative electrode current collector 36 is, for example, 5 μm to 25 μm, preferably 8 μm to 20 μm, and more preferably 8 μm to 15 μm. The thickness of the negative electrode active material layer 37 is, for example, 20 μm to 300 μm, preferably 30 μm to 250 μm, and more preferably 30 μm to 150 μm. By increasing the thickness of the negative electrode active material layer 37, the active material capacity per unit area can be increased, and the energy density of the battery 11 can be increased. By decreasing the thickness of the negative electrode active material layer 37, deterioration of battery characteristics (particularly, an increase in resistance value) due to repeated charge and discharge can be suppressed.
[0047] (Negative Electrode Structure 2) In the lithium secondary battery according to the present disclosure, the negative electrode is not limited to a coated electrode. 4 Ti 5 O 12 The negative electrode may be constructed using a sintered plate of LTO (hereinafter sometimes referred to as LTO). The LTO sintered plate has a structure in which a plurality of (i.e., a large number of) primary particles are bonded together. These primary particles are composed of LTO. LTO is typically known to have a spinel structure, but can also adopt other structures during charging and discharging. For example, LTO can be used to convert Li 4 Ti 5 O 12 (spinel structure) and Li 7 Ti 5 O 12 The reaction proceeds in the coexistence of two phases, i.e., the spinel structure and the LTO (rock salt structure). Therefore, the LTO is not limited to a spinel structure.
[0048] The primary particle size, which is the average particle size of the multiple primary particles that make up the LTO sintered body plate, may be 1.2 μm or less. It is preferably 0.02 to 1.2 μm, and more preferably 0.05 to 0.7 μm. The thickness of the LTO sintered body plate may be 10 to 290 μm. It is preferably 10 to 200 μm, more preferably 40 to 200 μm, even more preferably 40 to 175 μm, and particularly preferably 50 to 160 μm. The thicker the LTO sintered body plate, the easier it is to realize a battery with a high capacity and high energy density.
[0049] The LTO sintered body plate contains pores. By including pores, particularly open pores, in the LTO sintered body plate, when the LTO sintered body plate is incorporated into a battery as a negative electrode, it becomes easier for the electrolyte to penetrate into the LTO sintered body plate. As a result, lithium ion conductivity can be improved. The porosity of the LTO sintered body plate is, for example, 21 to 45%, more preferably 22 to 40%, and even more preferably 25 to 35%. Within these ranges, it is easy to achieve both lithium ion conductivity and electronic conductivity. Furthermore, in the LTO sintered body plate, the open pore ratio, which is the ratio of open pores to the total pores, may be 60% or more. It is more preferably 65% or more, even more preferably 70% or more, and particularly preferably 80% or more. The open pore ratio may be 100%. A large number of open pores makes it easier for the electrolyte to penetrate sufficiently into the sintered body plate, thereby improving lithium ion conductivity.
[0050] (Separator) The separator 23 is a sheet-like or thin-plate-like insulating member. The separator 23 is, for example, a single-layer separator formed from a resin. Examples of resins that can be used include polyimide, polyester (e.g., polyethylene terephthalate (PET)), and cellulose. The thickness of the separator 23 is, for example, 15 μm or more, preferably 18 μm or more, and more preferably 20 μm or more. The thickness of the separator 23 is, for example, 31 μm or less, preferably 28 μm or less, and more preferably 26 μm or less. By increasing the thickness of the separator, even if lithium dendrites (tree-like crystals of lithium) precipitate, short-circuiting between the positive electrode and the negative electrode due to lithium dendrites can be prevented. Furthermore, by reducing the thickness of the separator, the permeation of the electrolyte and lithium ions can be facilitated, thereby reducing the internal resistance of the battery 11.
[0051] The structure of the separator 23 may be changed to a known structure other than the above. For example, it may be a laminate of two or three or more layers of ceramic and resin. It may also be a microporous film made only of ceramic. The ceramic may be, for example, MgO, Al 2 O 3 , ZrO, SiC, Si 3 N 4, AlN and cogenerationlite, and preferably MgO, Al 2 O 3 and ZrO 2 At least one selected from the following.
[0052] (Electrolyte) The electrolyte 24 is a liquid obtained by adding an electrolyte and an additive to a solvent. For example, the electrolyte may be lithium hexafluorophosphate (LiPF 6 The electrolyte may be modified, for example, lithium borofluoride (LiBF 4 ) The concentration of the electrolytic solution 24 may be, for example, 1.0 to 8.0 mol / L. It is preferably 1.5 mol / L or more, more preferably 2.0 mol / L or more, even more preferably 4.0 mol / L or more, and even more preferably 5.0 mol / L or more. A preferred numerical range for the concentration of the electrolytic solution 24 is, for example, 1.5 mol / L to 8.0 mol / L, more preferably 2.0 mol / L to 8.0 mol / L, and even more preferably 4.0 mol / L to 5.0 mol / L.
[0053] The solvent of the electrolytic solution 24 is a non-aqueous solvent such as ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), γ-butyrolactone (GBL), methyl butyrate (MB), propyl acetate (PA), etc. The solvent may be, for example, a solvent containing EC and EMC.
[0054] (Thickness of Lithium Secondary Battery in High-Temperature and Reduced-Pressure Environments) In a lithium secondary battery according to the present disclosure, the ratio of the thickness of the exterior body 12 in a high-temperature, reduced-pressure environment to the thickness of the exterior body 12 in a room-temperature, normal-pressure environment is 1.05 or more and 2.63 or less. Specifically, the ratio of the thickness of the exterior body 12 at a temperature of 80°C and a pressure of 100 Pa to the thickness of the exterior body 12 at a temperature of 25°C and a pressure of 101,325 Pa is 1.05 or more and 2.63 or less. More preferably, the ratio of the thickness of the exterior body 12 at a temperature of 80°C and a pressure of 100 Pa to the thickness of the exterior body 12 at a temperature of 25°C and a pressure of 101,325 Pa is 1.05 or more and 1.50 or less.
[0055] The lithium secondary battery of the present disclosure will be described in more detail with reference to examples and comparative examples.
[0056] Example 1 A lithium secondary battery was fabricated according to the methods described in (1) to (3) below, and the obtained lithium secondary battery was evaluated according to the method described in (4).
[0057] In the following Examples and Comparative Examples, the viscosity of the slurry used in the preparation of the green sheets was measured using an LVT viscometer manufactured by Brookfield Co., Ltd. The doctor blade method was used to form the slurry on a PET film.
[0058] (1) Preparation of positive electrode (1a) LiCoO 2 Preparation of (LCO) green sheet Co was weighed so that the Li / Co molar ratio was 1.01. 3 O 4 Powder (manufactured by Seido Chemical Industry Co., Ltd.) and Li 2 CO 3 The powder (manufactured by Honjo Chemical Co., Ltd.) was mixed and then held at 780°C for 5 hours. The obtained powder was milled in a pot mill to a volume standard D 50 The resulting LCO powder (100 parts by weight), 100 parts by weight of a dispersion medium (toluene:isopropanol=1:1), 10 parts by weight of a binder (polyvinyl butyral: product number BM-2, manufactured by Sekisui Chemical Co., Ltd.), 4 parts by weight of a plasticizer (DOP: Di(2-ethylhexyl) phthalate, manufactured by Kurogane Kasei Co., Ltd.), and 2 parts by weight of a dispersant (product name Rheodol SP-O30, manufactured by Kao Corporation) were mixed together. The resulting mixture was stirred under reduced pressure to degas and the viscosity was adjusted to 4000 cP, thereby obtaining a LiCoO 2 A slurry was prepared. The prepared slurry was formed into a sheet on a PET film, and LiCoO 2 A green sheet was formed. LiCoO after drying 2 The thickness of the green sheet was 98 μm.
[0059] (1b) LiCoO 2 Preparation of sintered body plate LiCoO peeled from PET film2 The green sheet was cut into 50 mm square pieces with a cutter and placed at the center of a magnesia setter (90 mm square, 1 mm high) as the lower setter. 2 A porous magnesia setter was placed on the sheet as an upper setter. 2 The sheet was sandwiched between setters and placed in a 120 mm square alumina sheath (manufactured by Nikkato Corporation). At this time, the alumina sheath was not sealed, but was covered with a lid leaving a gap of 0.5 mm. The obtained laminate was heated to 600°C at a heating rate of 200°C / h and degreased for 3 hours, then heated to 920°C at 200°C / h and held for 4 hours, thereby performing firing. After firing, the temperature was lowered to room temperature and the fired body was removed from the alumina sheath. By these procedures, a 90 μm-thick LiCoO 2 The sintered plate was obtained as a positive electrode. The obtained positive electrode was cut into a rectangular shape of 9.75 mm × 18.15 mm square using a laser processing machine to obtain a chip-shaped positive electrode.
[0060] (2) Preparation of negative electrode (2a) Li 4 Ti 5 O 12 Preparation of (LTO) green sheet First, LTO powder (volume basis D 50 100 parts by weight of a 0.06 μm particle size (Sigma-Aldrich Japan LLC), 100 parts by weight of a dispersion medium (toluene:isopropanol = 1:1), 20 parts by weight of a binder (polyvinyl butyral: product number BM-2, Sekisui Chemical Co., Ltd.), 4 parts by weight of a plasticizer (DOP: Di(2-ethylhexyl) phthalate, Kurogane Kasei Co., Ltd.), and 2 parts by weight of a dispersant (product name Rheodol SP-O30, Kao Corporation) were mixed. The resulting negative electrode raw material mixture was stirred under reduced pressure to degas and the viscosity was adjusted to 4000 cP to prepare an LTO slurry. The prepared slurry was formed into a sheet on a PET film to form an LTO green sheet. The thickness of the LTO green sheet after drying was adjusted to 110 μm after firing.
[0061] (2b) Firing of LTO Green Sheet The obtained green sheet was cut into 25 mm squares using a utility knife and placed on an embossed zirconia setter. The green sheet on the setter was placed in an alumina sheath and held at 500°C for 5 hours, then heated at a rate of 200°C / h and fired at 800°C for 5 hours. A 100 nm thick Au film was formed as a current collecting layer by sputtering on the surface of the obtained LTO sintered body plate that had been in contact with the setter, and then laser-machined into a 9.12 mm x 17.52 mm rectangular shape.
[0062] (3) Assembly of Lithium Secondary Battery A lithium secondary battery 11, which is the lithium secondary battery shown in Fig. 1, was produced in the following procedure. An outline of the production process is shown in Fig. 4. Fig. 4 is a schematic diagram showing the assembly process of a lithium secondary battery.
[0063] Two aluminum laminate films (manufactured by Showa Denko Packaging, 61 μm thick, with a three-layer structure of polypropylene film / aluminum foil / nylon film) were prepared as exterior films 13 and 14. As shown in FIG. 4(1), one positive electrode active material plate 32 was laminated on one exterior film 13 via a positive electrode current collector 31 (aluminum foil with a thickness of 9 μm) to form a positive electrode assembly 41. At this time, the positive electrode current collector 31 was not fixed to the exterior film 13 with an adhesive. Note that a positive electrode tab terminal 15 was fixed to the positive electrode current collector 31 by welding in a manner extending from the positive electrode current collector 31. Meanwhile, a negative electrode active material layer 37 was laminated on the other exterior film 14 with a negative electrode current collector 36 (aluminum foil with a thickness of 9 μm) interposed therebetween to form a negative electrode assembly 42. At this time, the negative electrode current collector 36 was not fixed to the exterior film 14 with an adhesive. The negative electrode tab terminal 16 is fixed to the negative electrode current collector 36 by welding in a manner that it extends from the negative electrode current collector 36 .
[0064] As the separator 23, a cellulose membrane (manufactured by Nippon Kodo Paper Industries, Ltd., thickness 20 μm, density 0.47 g / cm 3) was prepared. As shown in FIG. 4(2), a positive electrode assembly 41, a separator 23, and a negative electrode assembly 42 were stacked in this order, with the positive electrode active material plate 32 and the negative electrode active material layer 37 facing the separator 23. A laminate 43 was obtained, in which both sides were covered with exterior films 13 and 14, and the peripheral portions of the exterior films 13 and 14 protruded beyond the outer edges of the battery element. The thickness of the battery element (positive electrode current collector 31, positive electrode active material plate 32, separator 23, negative electrode active material layer 37, and negative electrode current collector 36) constructed inside the laminate 43 was 0.33 mm. The size and shape were a rectangle measuring 1.3 cm x 2.2 cm.
[0065] 4(3), three sides of the obtained laminate 43 were sealed. This sealing was performed by heat-pressing the outer periphery of the laminate 43 at 200°C and 1.5 MPa for 15 seconds using a pressing tool (heat bar) adjusted to a sealing width of 2.0 mm, thereby heat-sealing the exterior films 13 and 14 (aluminum laminate films) together at the outer periphery.
[0066] As shown in FIG. 4(4), after sealing the three sides, the laminate 43 was placed in a vacuum dryer 44 to remove moisture and dry the adhesive.
[0067] Next, as shown in FIG. 4 (5), in a glove box 45, a gap was formed between the exterior films 13 and 14 on the remaining unsealed side of the laminate 43, the three outer edges of which were sealed, and an injection tool 46 was inserted into the gap to inject the electrolyte 24.
[0068] As shown in Figure 4 (6), one unsealed side was temporarily sealed using a simple sealer under a reduced pressure of 5 kPa absolute. The electrolyte was an organic solvent made by mixing ethylene carbonate (EC) and γ-butyrolactone (GBL) in a volume ratio of 1:3, and LiBF 4 was dissolved to a concentration of 1.5 mol / L.
[0069] As shown in FIG. 4(7), the temporarily sealed laminate 43 was subjected to an initial charge and then aged at 120° C. for 1 hour.
[0070] As shown in FIG. 4(8), after the aging, the outer peripheral portion of one sealed side (the end portion not including the battery element) was cut off to remove gas.
[0071] Next, as shown in FIG. 4 (9), the openings resulting from the removal of the temporary seals were sealed in a glove box 45 under a reduced pressure of 5 kPa absolute. This sealing was also performed by heat-pressing the outer periphery of the laminate 43 at 200°C and 1.5 MPa for 15 seconds to heat-seal the outer periphery of the exterior films 13 and 14. This resulted in a lithium secondary battery 11. The battery 11 was removed from the glove box 45, and excess outer periphery portions of the exterior films 13 and 14 were trimmed to adjust the shape of the battery 11. Thus, a lithium secondary battery 11 was obtained, in which the four outer edges of the battery element were sealed with a pair of exterior films 13 and 14 and the electrolyte 24 was injected. The resulting battery 11 was a rectangle measuring 27 mm x 17 mm and 0.40 mm (400 μm) thick.
[0072] (4) (Evaluation) (Measurement of Thickness of Exterior Body) Here, a method for measuring the thickness of the exterior body 12 will be briefly described. FIG. 5 is a schematic cross-sectional view showing a portion of a measuring device 51 used to measure the thickness of the exterior body 12. Referring to FIG. 5, first, a Pelger-type vacuum oven (Model BV-001, manufactured by Shibata Scientific Instruments Co., Ltd.) is prepared. Then, a dial gauge (manufactured by Mitutoyo Corporation) 52 is fixed on the Pelger-type vacuum oven using double-sided tape and polyimide tape. Then, at room temperature and normal pressure (normal temperature and normal pressure), polyimide sheets 54, 55, 56, and 57 are placed on a plate 53, and the battery 11 (exterior body 12) is placed on top of them. At this time, the tip 58 of the dial gauge 52 is positioned at the center of the battery 11. Here, the number of polyimide sheets 54, 55, 56, and 57 is adjusted so that the tip 58 contacts the battery 11, and the value of the dial gauge 52 when in contact is 0. After the adjustment of the dial gauge 52 is completed, the battery 11 is removed from the plate 53.
[0073] Next, the temperature of the Pelger type vacuum oven is set and the process waits until the set temperature (80° C.) is stabilized. At this time, the polyimide sheets 54, 55, 56, and 57 are also heated.
[0074] Next, place the battery 11 on the polyimide sheets 54, 55, 56, and 57 placed on the plate 53 and wait for two minutes. Adjust the number of polyimide sheets 54, 55, 56, and 57. At this time, position the tip 58 of the dial gauge 52 at the center of the battery 11.
[0075] Next, a peljar is placed over the container, and vacuuming (reducing pressure) is initiated. The value on the dial gauge 52 is read when the vacuum gauge reaches 100 Pa. The thickness of the exterior body 12 is determined by adding the value on the dial gauge 52 and the thickness of the exterior body 12 at room temperature and normal pressure. (Thickness of the exterior body 12 = (value on the dial gauge 52) + (thickness of the exterior body 12 at room temperature and normal pressure)).
[0076] If the needle of the dial gauge 52 swings too far and measurement is not possible, remove the polyimide sheets 54, 55, 56, and 57 placed under the battery 11 one by one and repeat the measurement until measurement is possible. Each time a polyimide sheet 54, 55, 56, or 57 is removed, the thickness of the exterior body 12 is calculated as (the value of the dial gauge 52) + (the thickness of the polyimide sheets 54, 55, 56, and 57 × the number of sheets removed) + (the thickness of the exterior body 12 at room temperature and normal pressure).
[0077] Furthermore, if measurement is not possible even when there are no polyimide sheets 54, 55, 56, 57 (when all polyimide sheets 54, 55, 56, 57 are removed), the value shall be equal to or greater than the value calculated by (maximum value of dial gauge 52) + (thickness of polyimide sheets 54, 55, 56, 57 x number of sheets removed) + (thickness of outer casing 12 at room temperature and normal pressure).
[0078] (Method for Evaluating Charge and Discharge) Charge and discharge were evaluated as follows. The lithium secondary battery was charged at a constant current of 0.2 C to the charge voltage value, and then charged at a constant voltage until the current reached 0.02 C. Then, it was discharged at a constant current of 0.5 C to the discharge voltage value, and the discharge capacity W0 at room temperature and normal pressure was measured. When measuring in a high-temperature environment or a reduced-pressure environment, the temperature of a Pelger-type vacuum oven was set and stabilized, and then the battery 11 was placed on a plate, covered with a Pelger, and the pressure was reduced to 100 Pa. Then, charge and discharge evaluation was performed in the same manner as at room temperature and normal pressure, and the discharge capacity W1 at the reduced pressure was measured. The discharge capacity retention rate (%) was calculated by dividing the discharge capacity W1 by the discharge capacity W0 and converting the result into a percentage.
[0079] A lithium secondary battery was obtained in the same manner as in Example 1, except that an organic solvent in which ethylene carbonate (EC) and γ-butyrolactone (GBL) were mixed in a volume ratio of 7:3 was used as the electrolyte solution 24. Evaluation was carried out in the same manner as in Example 1.
[0080] Example 3 A lithium secondary battery was obtained in the same manner as in Example 1, except that the positive electrode current collector 31 was fixed to the exterior film 13 with an adhesive, and the negative electrode current collector 36 was fixed to the exterior film 14 with an adhesive. The adhesive used was composed of a mixed resin of an acid-modified polyolefin resin and an epoxy resin. Specifically, Hardlen (registered trademark) (manufactured by Toyobo Co., Ltd.) was used as the adhesive. Evaluation was performed in the same manner as in Example 1.
[0081] Example 4 An organic solvent in which ethylene carbonate (EC) and γ-butyrolactone (GBL) were mixed in a volume ratio of 7:3 was used as the electrolyte solution 24, and LiBF 4 A lithium secondary battery was obtained in the same manner as in Example 1, except that a solution in which the above was dissolved to a concentration of 4.0 mol / L was used. Evaluation was carried out in the same manner as in Example 1.
[0082] Example 5 The same lithium secondary battery as in Example 4 was used, and evaluation was carried out in the same manner except that the evaluation temperature was 120°C.
[0083] Example 6: An organic solvent in which ethylene carbonate (EC) and propylene carbonate (PC) were mixed in a volume ratio of 3:1 was used as the electrolyte solution 24. 6 A lithium secondary battery was obtained in the same manner as in Example 1, except that a solution in which the above was dissolved to a concentration of 1.0 mol / L was used. Evaluation was carried out in the same manner as in Example 1.
[0084] Example 7 A lithium secondary battery was obtained in the same manner as in Example 1, except that an organic solvent in which sulfolane (SL) and γ-butyrolactone (GBL) were mixed in a volume ratio of 7:3 was used as the electrolyte solution 24 and a plate-shaped electrode was used as the negative electrode 22. Evaluation was performed in the same manner as in Example 1.
[0085] Example 8 An organic solvent in which ethylene carbonate (EC) and γ-butyrolactone (GBL) were mixed in a volume ratio of 7:3 was used as the electrolyte solution 24, and LiBF 4 A lithium secondary battery was obtained in the same manner as in Example 1, except that a solution in which the above was dissolved to a concentration of 4.0 mol / L was used and a plate electrode was used as the negative electrode 22. Evaluation was carried out in the same manner as in Example 1.
[0086] Example 9: As the electrolyte 24, an organic solvent in which ethylene carbonate (EC) and γ-butyrolactone (GBL) were mixed in a volume ratio of 7:3 was used, and LiBF 4 A lithium secondary battery was obtained in the same manner as in Example 1, except that a solution in which the above was dissolved to a concentration of 4.0 mol / L was used and a coated electrode was used as the positive electrode 21. Evaluation was carried out in the same manner as in Example 1.
[0087] Example 10: As the electrolyte 24, an organic solvent in which sulfolane (SL) and γ-butyrolactone (GBL) were mixed in a volume ratio of 4:1 was used, and LiBF 4 A lithium secondary battery was obtained in the same manner as in Example 1, except that a solution in which the above was dissolved to a concentration of 5.0 mol / L was used. Evaluation was carried out in the same manner as in Example 1.
[0088] Comparative Example 1: As the electrolyte 24, an organic solvent in which diethyl carbonate (DEC), propylene carbonate (PC), and ethylene carbonate (EC) were mixed in a volume ratio of 5:1:1 was used. 4 A lithium secondary battery was obtained in the same manner as in Example 1, except that a solution in which the above was dissolved to a concentration of 1.0 mol / L was used and a coated electrode was used as the positive electrode 21. Evaluation was carried out in the same manner as in Example 1.
[0089] Comparative Example 2: An organic solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 1:3 was used as the electrolyte solution 24. 4 A lithium secondary battery was obtained in the same manner as in Example 1, except that a solution in which the above was dissolved to a concentration of 1.0 mol / L was used and a coated electrode was used as the positive electrode 21. Evaluation was carried out in the same manner as in Example 1.
[0090] The evaluation results of the lithium secondary batteries of Examples 1 to 10 and Comparative Examples 1 and 2 are summarized in Table 1.
[0091]
[0092] As shown in Table 1, lithium secondary batteries in which the ratio of the thickness of the exterior body 12 at a temperature of 80°C and a pressure of 100 Pa to the thickness of the exterior body 12 at a temperature of 25°C and a pressure of 101,325 Pa is 1.05 or more and 2.63 or less have a discharge capacity retention rate of 70% or more and 98% or less even in a high-temperature environment and a reduced-pressure environment, specifically, an environment at a temperature of 80°C and a pressure of 100 Pa. That is, the lithium secondary batteries of Examples 1 to 9 can maintain good characteristics even in a high-temperature environment and a reduced-pressure environment. Note that, in Examples 3, 7, and 8, the occurrence of wrinkles in the exterior material can be suppressed.
[0093] On the other hand, the lithium secondary batteries of Comparative Examples 1 and 2, which have a thickness ratio greater than 2.63, have a discharge capacity retention rate of 5% or less. Such lithium secondary batteries cannot maintain good characteristics in high-temperature and reduced-pressure environments.
[0094] It should be understood that the embodiments disclosed herein are illustrative in all respects and are not limiting in any respect. The scope of the present invention is defined not by the above description but by the claims, and it is intended to include all modifications within the meaning and scope of the claims.
[0095] REFERENCE SIGNS LIST 11 Lithium secondary battery (battery), 12 Exterior body, 13, 14 Exterior film, 15 Positive electrode tab terminal, 16 Negative electrode tab terminal, 17 Sealed space, 21 Positive electrode, 22 Negative electrode, 23 Separator, 24 Electrolyte, 25, 26 Metal foil, 27, 28 Resin layer, 31 Positive electrode current collector, 32 Positive electrode active material plate, 33 Conductive bonding layer, 34 Positive electrode bonding layer, 36 Negative electrode current collector, 37 Negative electrode active material layer, 38 Negative electrode bonding layer, 41 Positive electrode assembly, 42 Negative electrode assembly, 43 Laminate, 44 Vacuum dryer, 45 Glove box, 46 Injection tool, 51 Measuring device, 52 Dial gauge, 53 Plate, 54, 55, 56, 57 Polyimide sheet, 58 Tip.
Claims
1. A pouch-type lithium secondary battery comprising: a positive electrode layer formed of a sintered lithium composite oxide; a negative electrode layer; a separator interposed between the positive electrode layer and the negative electrode layer; an electrolytic solution containing an electrolyte and a solvent impregnated into the positive electrode layer, the negative electrode layer, and the separator; and an exterior body having an enclosed space in which the positive electrode layer, the negative electrode layer, the separator, and the electrolytic solution are accommodated, wherein the ratio of a thickness of the exterior body at a temperature of 80° C. and a pressure of 100 Pa to a thickness of the exterior body at a temperature of 25° C. and a pressure of 101,325 Pa in the thickness direction of the positive electrode layer is 1.05 or more and 2.63 or less.
2. The lithium secondary battery according to claim 1, wherein the positive electrode layer is a plate electrode, and the negative electrode layer is a plate electrode.
3. The lithium secondary battery according to claim 1 or 2, wherein the solvent is a mixed liquid solvent containing a first substance which is an ester having a carbonate and a second substance which is an ester different from the first substance and has a carbonate or a lactone, and the volume ratio of the first substance to the second substance is within the range of 1:10 or more and 10:1 or less.
4. The lithium secondary battery according to claim 1 or 2, wherein the electrolyte has a concentration of 2.0 mol / L or more and 8.0 mol / L or less.
5. A lithium secondary battery as described in claim 1 or claim 2, further comprising an adhesive that is made of a mixed resin of an acid-modified polyolefin resin and an epoxy resin and that bonds at least one of the positive electrode layer or the negative electrode layer to the exterior body in the sealed space.
6. The lithium secondary battery according to claim 1, further comprising an adhesive composed of a mixed resin of an acid-modified polyolefin resin and an epoxy resin, which bonds at least one of the positive electrode layer or the negative electrode layer to the exterior body in the sealed space, wherein the positive electrode layer is a plate electrode, the negative electrode layer is a plate electrode or a coated electrode, the solvent is a mixed solvent containing sulfolane and γ-butyrolactone, the volume ratio of the sulfolane to the γ-butyrolactone is 7:3 or more and 4:1 or less, and the concentration of the electrolyte is 1.5 mol / L or more and 5.0 mol / L or less.
Citation Information
Patent Citations
Nonaqueous secondary battery
JP2000331715A
Electro chemical device
JP2002008629A
Nonaqueous electrolyte secondary battery
JP2002033117A
Positive electrode active material for lithium ion secondary cell and manufacturing method therefor
JP2002352802A
Positive active material for lithium ion secondary battery
JP2003022805A
Cited By
Adhesive composition, reinforcing film, and current collector
WO2026225424A1