Thermosetting resin, cured product thereof, and thermosetting composition

The thermosetting resin with a specific linear copolymer composition addresses the balance of dielectric properties and glass transition temperature, achieving low melt viscosity and improved moldability for high-frequency communication materials.

WO2024203866A1PCT designated stage expired Publication Date: 2024-10-03DKS CO LTD

Patent Information

Application Number
PCT/JP2024/011329
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional thermosetting resins often fall short in achieving a balance between dielectric properties and glass transition temperature, while also exhibiting high melt viscosity and poor processability.

Method used

A thermosetting resin with a linear copolymer structure comprising repeating units of monovinyl aromatic, divinyl aromatic, and aromatic ring-fused cyclic olefin compounds, optimized to achieve low melt viscosity and improved dielectric properties, is developed. The resin includes a specific composition of styrene, divinylbenzene, and acenaphthylene units, which are polymerized using a radical initiator to ensure a linear chain structure without branching, enhancing moldability and dielectric performance.

Benefits of technology

The resulting thermosetting resin achieves excellent dielectric properties, including low dielectric loss tangent and constant, while maintaining a high glass transition temperature and low melt viscosity, making it suitable for high-frequency communication materials and improving processability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

Provided is a thermosetting resin that can achieve a balance between dielectric characteristics and glass transition temperature, and that has a low melt viscosity. A thermosetting resin according to an embodiment is a linear copolymer comprising a repeating unit corresponding to a monovinyl aromatic compound, a repeating unit corresponding to a divinyl aromatic compound, and a repeating unit corresponding to an aromatic ring-condensed cyclic olefin compound.
Need to check novelty before this filing date? Find Prior Art

Description

Thermosetting resin, its cured product, and thermosetting composition

[0001] FIELD OF THE INVENTION The present invention relates to a thermosetting resin and a cured product thereof, and also to a thermosetting composition containing the thermosetting resin.

[0002] In recent years, electronic devices have become smaller and more powerful, and as a result, the performance requirements for the various materials used in them have increased. For example, there is a demand for printed circuit board materials with low dielectric loss tangents that can be used for high-frequency communications.

[0003] Patent Document 1 discloses a thermosetting resin composition having excellent dielectric properties, heat resistance, adhesion, and moisture resistance, which contains a copolymer containing an acenaphthylene-based structural unit and a hydroxystyrene-based structural unit, a compound having at least two epoxy groups in one molecule, and a curing agent. Patent Document 1 discloses a copolymer of styrene, p-t-butoxystyrene, divinylbenzene, and acenaphthylene as a specific example of the copolymer, but the copolymer has a branched chain.

[0004] Patent Document 2 discloses a copolymer containing a structural unit derived from a divinyl aromatic compound, a structural unit derived from a monovinyl aromatic compound, and a structural unit derived from a cycloolefin compound, as a copolymer that provides a curable composition excellent in heat resistance, compatibility, dielectric properties, moist heat reliability, and thermal oxidative degradation resistance. In Patent Document 2, the copolymer is polymerized using a mixed solution of a divinyl aromatic compound, a monovinyl aromatic compound, and a cycloolefin compound, and therefore the obtained copolymer has a branched chain.

[0005] JP 2001-192539 A JP 2018-039995 A

[0006] Conventional thermosetting resins are not necessarily satisfactory in terms of dielectric properties, and even those with excellent dielectric properties have problems such as a low glass transition temperature or high melt viscosity, which makes them poor in processability.

[0007] In view of the above, an object of an embodiment of the present invention is to provide a thermosetting resin that can achieve both dielectric properties and a glass transition temperature and has a low melt viscosity.

[0008] The present invention includes the following embodiments. [1] A thermosetting resin that is a linear copolymer having a repeating unit corresponding to a monovinyl aromatic compound, a repeating unit corresponding to a divinyl aromatic compound, and a repeating unit corresponding to an aromatic ring-fused cyclic olefin compound. [2] The thermosetting resin according to [1], wherein the content of the repeating unit corresponding to the aromatic ring-fused cyclic olefin compound is 5 to 80 mol % based on 100 mol % of all repeating units. [3] The linear copolymer has a repeating unit represented by general formula (1): R 1 -N=N-R 2 and R in the general formula (1) 1 and R 2 each independently represent a monovalent saturated hydrocarbon group or a monovalent aromatic hydrocarbon group. [4] The thermosetting resin according to any one of [1] to [3], wherein the total content of repeating units corresponding to the monovinyl aromatic compound, repeating units corresponding to the divinyl aromatic compound, and repeating units corresponding to the aromatic-ring-fused cyclic olefin compound is 80 mol % or more, based on 100 mol % of all repeating units. [5] The thermosetting resin according to any one of [1] to [4], wherein the aromatic-ring-fused cyclic olefin compound has 3 or less rings. [6] A cured product obtained by curing the thermosetting resin according to any one of [1] to [5]. [7] A thermosetting composition comprising the thermosetting resin according to any one of [1] to [5]. [8] The thermosetting composition according to [7], which is a printed circuit board material.

[0009] According to an embodiment of the present invention, a thermosetting resin can be obtained that can achieve both dielectric properties and glass transition temperature and has a low melt viscosity.

[0010] The thermosetting resin according to this embodiment is a copolymer having a repeating unit corresponding to (A) a monovinyl aromatic compound, a repeating unit corresponding to (B) a divinyl aromatic compound, and a repeating unit corresponding to (C) an aromatic ring-fused cyclic olefin compound.

[0011] The repeating unit corresponding to the monovinyl aromatic compound of (A) (hereinafter also referred to as "monovinyl aromatic compound unit") is a constituent unit of the copolymer, and is a constituent unit having a structure formed by addition polymerization of a monovinyl aromatic compound as a monomer. The repeating unit is not necessarily limited to one obtained by polymerization using the monovinyl aromatic compound, as long as it has a structure corresponding to the monovinyl aromatic compound, and may be one that has been further reacted after polymerization to form a structure corresponding to the monovinyl aromatic compound.

[0012] Examples of the monovinyl aromatic compound unit include a repeating unit having a structure in which the vinyl group of a monovinyl aromatic compound becomes a single bond through addition polymerization, as represented by the following general formula (2).

[0013] In formula (2), R 3 represents a monovalent aromatic hydrocarbon group having 6 to 30 carbon atoms. 3 is a monovalent aromatic hydrocarbon group having 6 to 30 carbon atoms (more preferably 6 to 20 carbon atoms) selected from the group consisting of a phenyl group which may have a substituent, a biphenylyl group which may have a substituent, a naphthyl group which may have a substituent, and a terphenylyl group which may have a substituent. 3 When R has a substituent such as an alkyl group, the number of carbon atoms in R includes the number of carbon atoms in the substituent. 3 The total number of carbon atoms.

[0014] The monovinyl aromatic compound forming such a repeating unit may be any aromatic compound having one vinyl group, and examples thereof include vinyl aromatic compounds such as styrene, vinylnaphthalene, and vinylbiphenyl, and nuclear alkyl-substituted vinyl aromatic compounds such as alkylstyrenes (e.g., o-methylstyrene, m-methylstyrene, p-methylstyrene, o-ethylstyrene, m-ethylstyrene, and p-ethylstyrene), dialkylstyrenes (e.g., 3,5-dimethylstyrene, 2,5-dimethylstyrene, and 2,5-diethylstyrene), alkylvinylbiphenyls (e.g., ethylvinylbiphenyl), and alkylvinylnaphthalenes (e.g., ethylvinylnaphthalene), and any of these may be used alone or in combination of two or more.

[0015] In one embodiment, the monovinyl aromatic compound preferably contains at least one repeating unit (A1) selected from the group consisting of styrene, vinylnaphthalene, vinylbiphenyl, alkylstyrene, dialkylstyrene, alkylvinylbiphenyl, and alkylvinylnaphthalene. In this case, the amount of repeating units corresponding to the at least one repeating unit (A1) in 100 mol% of the monovinyl aromatic compound units is preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 90 mol% or more, and may even be 100 mol%.

[0016] In one embodiment, the monovinyl aromatic compound preferably contains styrene. In this case, the amount of repeating units corresponding to styrene (hereinafter also referred to as "styrene units") in 100 mol% of the monovinyl aromatic compound units is preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 90 mol% or more, and may be 100 mol%.

[0017] The repeating unit corresponding to the divinylaromatic compound (B) (hereinafter also referred to as "divinylaromatic compound unit") is a structural unit of the copolymer, and is a structural unit having a structure with one vinyl group, formed by addition polymerization of a divinylaromatic compound as a monomer. The repeating unit is not necessarily limited to one obtained by polymerization using the divinylaromatic compound, as long as it has a structure corresponding to the divinylaromatic compound, and may be one that has been further reacted after polymerization to form a structure corresponding to the divinylaromatic compound.

[0018] Examples of the divinyl aromatic compound unit include a repeating unit having a structure in which one vinyl group of the divinyl aromatic compound is converted into a single bond by addition polymerization, as represented by the following general formula (3).

[0019] In formula (3), R 4 represents a divalent aromatic hydrocarbon group having 6 to 30 carbon atoms. 4 is a divalent aromatic hydrocarbon group having 6 to 30 carbon atoms (more preferably 6 to 20 carbon atoms) selected from the group consisting of a phenylene group which may have a substituent, a biphenyldiyl group which may have a substituent, a naphthylene group which may have a substituent, and a terphenyldiyl group which may have a substituent. 4 When R has a substituent such as an alkyl group, the number of carbon atoms in R includes the number of carbon atoms in the substituent. 4 The total number of carbon atoms.

[0020] The divinyl aromatic compound forming such a repeating unit may be any aromatic compound having two vinyl groups, such as divinylbenzene (including each positional isomer or a mixture thereof), divinylnaphthalene (including each positional isomer or a mixture thereof), and divinylbiphenyl (including each positional isomer or a mixture thereof), and these may be used alone or in combination of two or more.

[0021] In one embodiment, the divinylaromatic compound preferably contains at least one repeating unit (B1) selected from the group consisting of divinylbenzene, divinylnaphthalene, and divinylbiphenyl. In this case, the amount of repeating units corresponding to the at least one repeating unit (B1) in 100 mol% of divinylaromatic compound units is preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 90 mol% or more, and may be 100 mol%.

[0022] In one embodiment, the divinylaromatic compound preferably contains divinylbenzene (m-isomer, p-isomer, or a mixture of positional isomers thereof). In this case, the amount of repeating units corresponding to divinylbenzene (hereinafter also referred to as "divinylbenzene units") in 100 mol% of divinylaromatic compound units is preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 90 mol% or more, and may be 100 mol%.

[0023] The repeating unit corresponding to the aromatic ring-fused cyclic olefin compound (C) (hereinafter also referred to as "cyclic olefin unit") is a constituent unit of the copolymer, and is a constituent unit having a structure formed by addition polymerization of an aromatic ring-fused cyclic olefin compound as a monomer. The repeating unit is not necessarily limited to one obtained by polymerization using the aromatic ring-fused cyclic olefin compound, as long as it has a structure corresponding to the aromatic ring-fused cyclic olefin compound, and may be one that has been further reacted after polymerization to form a structure corresponding to the aromatic ring-fused cyclic olefin compound.

[0024] An aromatic ring-fused cyclic olefin compound is a cyclic olefin compound in which an aromatic ring is fused, and more specifically, a compound having a fused ring of an aliphatic ring having a carbon-carbon double bond and an aromatic ring. The condensation may be ortho-condensation or ortho-peri-condensation. Examples of aromatic ring-fused cyclic olefin compounds include indene-based compounds, acenaphthylene-based compounds, phenalene-based compounds, acephenanthrylene-based compounds, aceanthrylene-based compounds, benzofuran-based compounds, and benzothiophene-based compounds, and any one or more of these may be used in combination. Among these, aromatic ring-fused cyclic olefin compounds are preferably those having three or fewer rings. Specifically, compounds having two rings include indene-based compounds, benzofuran-based compounds, and benzothiophene-based compounds; and compounds having three rings include acenaphthylene-based compounds and phenalene-based compounds, and more preferably indene-based compounds and / or acenaphthylene-based compounds.

[0025] In one embodiment, the aromatic ring-fused cyclic olefin compound preferably contains at least one compound (C1) selected from the group consisting of an indene-based compound, an acenaphthylene-based compound, a phenalene-based compound, an acephenanthrylene-based compound, an aceanthrylene-based compound, a benzofuran-based compound, and a benzothiophene-based compound. In this case, the amount of repeating units corresponding to the at least one compound (C1) in 100 mol% of cyclic olefin units is preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 90 mol% or more, and may be 100 mol%.

[0026] The indene-based compound may be, for example, at least one selected from the group consisting of indene, alkylindene, halogenated indene, arylindene, and alkoxyindene.

[0027] The acenaphthylene-based compound may be, for example, at least one selected from the group consisting of acenaphthylene, alkylacenaphthylene, halogenated acenaphthylene, arylacenaphthylene, and alkoxyacenaphthylene.

[0028] The phenalene-based compounds, acephenanthrylene-based compounds, aceanthrylene-based compounds, benzofuran-based compounds, and benzothiophene-based compounds include phenalene, acephenanthrylene, aceanthrylene, benzofuran, and benzothiophene, as well as compounds having the same substituents as the above-mentioned indene-based compounds.

[0029] In one embodiment, the cyclic olefin unit includes a repeating unit represented by the following general formula (4).

[0030] In formula (4), R 5 and R 6 each independently represents an alkyl group having 1 to 20 carbon atoms, a halogen atom, an aryl group having 6 to 20 carbon atoms, or an alkoxy group having 1 to 20 carbon atoms. m and n each independently represent an integer of 0 to 3. When m and n are 2 or more, R 5 and R 6 may be the same or different.

[0031] The aromatic ring-fused cyclic olefin compound forming the repeating unit of formula (4) is an acenaphthylene-based compound represented by the following general formula (5). R in formula (5) 5 , R 6 , m and n are R in formula (4). 5 , R 6 , m and n.

[0032] In one embodiment, the aromatic ring-fused cyclic olefin compound preferably contains an acenaphthylene-based compound represented by the above formula (5), more preferably acenaphthylene. In this case, the amount of the repeating unit represented by formula (4) (preferably a repeating unit corresponding to acenaphthylene (hereinafter also referred to as "acenaphthylene unit")) in 100 mol% of cyclic olefin units is preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 90 mol% or more, and may be 100 mol%.

[0033] The thermosetting resin according to this embodiment is a linear copolymer having the above three repeating units. The linear structure causes entanglement of molecular chains, improving moldability. Here, linear refers to a structure in which the repeating units constituting the copolymer are linked together in a one-dimensional chain, and does not have a cross-linked structure.

[0034] In the thermosetting resin, the monovinyl aromatic compound units, divinylaromatic compound units, and cyclic olefin units may be arranged in a regular or random order, and the thermosetting resin is preferably a random copolymer in which the monovinyl aromatic compound units, divinylaromatic compound units, and cyclic olefin units are arranged randomly.

[0035] In addition to the monovinyl aromatic compound unit, the divinyl aromatic compound unit, and the cyclic olefin unit, the thermosetting resin may contain repeating units corresponding to other monomers, such as trivinyl aromatic compounds, trivinyl aliphatic compounds, divinyl aliphatic compounds, and monovinyl aliphatic compounds, as long as the effects of the other monomers are not impaired.

[0036] In the thermosetting resin, the content of the monovinyl aromatic compound unit is not particularly limited, but is preferably 15 to 90 mol% of the total repeating units constituting the copolymer, where 100 mol% is the total repeating units. A content of 15 mol% or more provides an excellent effect of reducing melt viscosity. The content of the monovinyl aromatic compound unit is more preferably 30 to 80 mol%, even more preferably 40 to 75 mol%, and even more preferably 50 to 70 mol%. Note that, in this specification, 100 mol% of all repeating units does not include structures derived from the polymerization initiator present at the terminals of the copolymer.

[0037] In the thermosetting resin, the content of the divinylaromatic compound unit is not particularly limited, but is preferably 3 to 30 mol% relative to 100 mol% of all repeating units constituting the copolymer. A content of 3 mol% or more can enhance thermosetting properties to obtain a good cured product and can also improve the glass transition temperature. The content of the divinylaromatic compound unit is more preferably 5 to 25 mol%, even more preferably 8 to 22 mol%, and even more preferably 10 to 20 mol%.

[0038] In the thermosetting resin, the content of the cyclic olefin unit is not particularly limited, but is preferably 5 to 80 mol% relative to 100 mol% of all repeating units constituting the copolymer. A content of 5 mol% or more provides an excellent effect of improving the glass transition temperature. A content of 80 mol% or less provides an excellent effect of reducing the melt viscosity. The content of the cyclic olefin unit is more preferably 7 to 50 mol%, even more preferably 8 to 35 mol%, and even more preferably 10 to 30 mol%.

[0039] The total content of the monovinyl aromatic compound units, divinyl aromatic compound units, and cyclic olefin units is preferably 80 mol % or more, more preferably 90 mol % or more, and may be 100 mol %, based on 100 mol % of all repeating units constituting the copolymer.

[0040] In one embodiment, the thermosetting resin is preferably a copolymer having a repeating unit represented by the above formula (2) (preferably a styrene unit), a repeating unit represented by the above formula (3) (preferably a divinylbenzene unit), and a repeating unit represented by the above formula (4) (preferably an acenaphthylene unit). In this case, the thermosetting resin preferably contains each repeating unit as follows, with the total repeating units constituting the copolymer being 100 mol %. In this case, the thermosetting resin may contain repeating units (A), (B), or (C) other than the repeating units. Repeating units represented by formula (2) (preferably a styrene unit): 15 to 90 mol %, preferably 30 to 80 mol %, more preferably 40 to 75 mol %, and even more preferably 50 to 70 mol %. Repeating units represented by formula (3) (preferably a divinylbenzene unit): 3 to 30 mol %, preferably 5 to 25 mol %, more preferably 8 to 22 mol %, and even more preferably 10 to 20 mol %. Repeating units represented by formula (4) (preferably acenaphthylene units): 5 to 80 mol %, preferably 7 to 50 mol %, more preferably 8 to 35 mol %, and even more preferably 10 to 30 mol %.

[0041] The thermosetting resin may have at least one of a structure derived from a polymerization initiator represented by the following general formula (1) or a structure derived from a polymerization initiator represented by the following general formula (6) at the end of the linear copolymer. The polymerization initiator represented by formula (1) is an azo initiator that does not have a cyano group, unlike azobisisobutyronitrile (AIBN), a general-purpose azo initiator. The polymerization initiator represented by formula (6) is an organic peroxide such as a dialkyl peroxide. Among these, the use of the polymerization initiator represented by formula (1) can impart better dielectric properties. R 1 -N=N-R 2 (1) R 7 -O-O-R 8 (6)

[0042] In formula (1) and formula (6), R 1 , R 2 , R 7 and R 8each independently represents a monovalent saturated hydrocarbon group or a monovalent aromatic hydrocarbon group, and does not contain a heteroatom. The number of carbon atoms in the saturated hydrocarbon group is not particularly limited, but is preferably 1 to 23, and more preferably 4 to 13. The number of carbon atoms in the aromatic hydrocarbon group is not particularly limited, but is preferably 6 to 23, and more preferably 6 to 13.

[0043] The saturated hydrocarbon group may be a branched or straight-chain saturated aliphatic hydrocarbon group (alkyl group) or a saturated alicyclic hydrocarbon group. Specific examples of the saturated hydrocarbon group include alkyl groups such as a tert-butyl group, a tert-pentyl group, a tert-hexyl group, and a 1,1,3,3-tetramethylbutyl group, and saturated alicyclic hydrocarbon groups such as a cyclohexyl group.

[0044] Specific examples of aromatic hydrocarbon groups include aryl groups such as phenyl, tolyl, and naphthyl, and aralkyl groups such as cumyl, benzyl, and phenethyl.

[0045] In one embodiment, R 1 , R 2 , R 7 and R 8 may each independently be a group represented by the following general formula (7):

[0046] In formula (7), R 9 , R 10 and R 11 each independently represents a monovalent saturated hydrocarbon group or a monovalent aromatic hydrocarbon group. 9 represents a monovalent saturated hydrocarbon group having 1 to 20 carbon atoms (more preferably 1 to 10 carbon atoms) or a monovalent aromatic hydrocarbon group having 6 to 20 carbon atoms (more preferably 6 to 10 carbon atoms); R 10 and R 11 represents a methyl group. 9 , R 10 and R 11 (Preferably R 9The saturated hydrocarbon group for R may be branched or linear, and examples thereof include alkyl groups such as methyl, ethyl, propyl, butyl, heptyl, isopropyl, tert-butyl, and 2,2-dimethylpropyl, and saturated alicyclic hydrocarbon groups such as cyclohexyl. 9 , R 10 and R 11 (Preferably R 9 Examples of the aromatic hydrocarbon group for ) include a phenyl group, a tolyl group, and a naphthyl group.

[0047] When a vinyl copolymer is synthesized by radical polymerization using these polymerization initiators, both ends of the obtained vinyl copolymer usually have a structure derived from the polymerization initiator. 1 - and / or R 2 A copolymer having R- at both ends is obtained. 1 - is also fine, both R 2 - is also acceptable, and one end is R 1 - and the other end is R 2 On the other hand, when polymerization is carried out using the polymerization initiator of the above formula (6), R 7 O- and / or R 8 A copolymer having O- at both ends is obtained. That is, both ends of the copolymer are R 7 O- is also acceptable, and both are R 8 O-, one end is R 7 O- and the other end is R 8 O- is also acceptable.

[0048] The weight-average molecular weight Mw of the thermosetting resin is not particularly limited and may be, for example, 1,000 to 100,000, 2,000 to 50,000, or 3,000 to 20,000. Having a weight-average molecular weight Mw of 1,000 or more reduces the concentration of terminal groups derived from the polymerization initiator, thereby improving dielectric properties. Furthermore, having a weight-average molecular weight Mw of 100,000 or less reduces the melt viscosity. Here, the weight-average molecular weight Mw is the weight-average molecular weight in terms of polystyrene measured by gel permeation chromatography (GPC).

[0049] The method for producing the thermosetting resin is not particularly limited. In a preferred embodiment of the method for synthesizing a linear copolymer, a vinylbenzyl phosphonium salt, a monovinyl aromatic compound, and an aromatic ring-fused cyclic olefin compound are copolymerized using at least one of the polymerization initiators represented by the above formula (1) and the polymerization initiators represented by the formula (6), and the resulting copolymer is reacted with formaldehyde. However, the method is not limited to this method.

[0050] As the vinylbenzyl phosphonium salt, it is preferable to use a vinylbenzyl phosphonium halide.The phosphonium group in the vinylbenzyl phosphonium salt may be, for example, a quaternary phosphonium group such as a trialkyl phosphonium, a triaryl phosphonium, or a triaralkyl phosphonium.In addition, the halogen atom that forms a salt with the phosphonium group may be, for example, chlorine, bromine, or the like.

[0051] The vinylbenzyl phosphonium salt can be copolymerized with a monovinyl aromatic compound and an aromatic ring-fused cyclic olefin compound by a known vinyl polymerization method.By using the radical polymerization initiator represented by the above formula (1) and / or formula (6) as the polymerization initiator, a copolymer having a repeating unit derived from the vinylbenzyl phosphonium salt, a repeating unit derived from the monovinyl aromatic compound, and a repeating unit derived from the aromatic ring-fused cyclic olefin compound can be obtained.During the polymerization, a chain transfer agent can be added to adjust the molecular weight of the copolymer.

[0052] The copolymer thus obtained can be reacted with formaldehyde by the well-known Wittig reaction, in which the copolymer is treated with a base and then reacted with formaldehyde, thereby removing the phosphonium group and introducing a vinyl group.

[0053] In this production method, since the vinylbenzyl phosphonium salt is monovinyl in the copolymerization step, a linear copolymer without branches can be obtained, and since a vinyl group is introduced into the repeating unit derived from the vinylbenzyl phosphonium salt after copolymerization, a linear copolymer without branches can be obtained, although it has a repeating unit corresponding to the divinyl aromatic compound.

[0054] The thermosetting composition according to this embodiment contains the thermosetting resin. The content of the thermosetting resin in the thermosetting composition is not particularly limited as long as the composition has the property of being cured by heat. For example, the content may be 1 to 99% by mass or 10 to 95% by mass relative to 100% by mass of the solid content of the thermosetting composition (this is the amount excluding the organic solvent when the organic solvent described below is contained, and the amount of the entire composition when the organic solvent is not contained).

[0055] In addition to the above-mentioned thermosetting resin, the thermosetting composition may contain various components such as other thermosetting resins (thermosetting crosslinking agents), thermoplastic resins, fillers, flame retardants, curing accelerators, polymerization initiators, antifoaming agents, heat stabilizers, antistatic agents, ultraviolet absorbers, colorants such as dyes and pigments, lubricants, and dispersants.

[0056] The thermosetting composition may contain an organic solvent to adjust its viscosity, or may be a solution containing the thermosetting resin. The organic solvent used may be one that can dissolve the thermosetting resin, and examples thereof include ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone, esters such as ethyl acetate, propyl acetate, and butyl acetate, amides such as dimethylacetamide and dimethylformamide, and aromatic hydrocarbons such as toluene and xylene. These may be used alone or in combination of two or more.

[0057] The thermosetting resin or thermosetting composition of this embodiment has vinyl groups in the molecular chain of the copolymer, allowing crosslinking by polymerization and producing a cured product by thermosetting. The cured product has low dielectric loss tangent and dielectric constant, resulting in excellent dielectric properties, and can be used in electronic materials such as printed circuit board materials and semiconductor encapsulation materials. In other words, the thermosetting composition of one embodiment is a thermosetting composition for electronic materials.

[0058] Examples of the printed circuit board material include rigid printed circuit board materials such as single-sided boards, double-sided boards, multilayer boards, and build-up boards, as well as film- or sheet-like flexible printed circuit board materials. In addition, because of their excellent dielectric properties, they are suitably used as high-frequency board materials for use in high-frequency communication devices.

[0059] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0060] <Measurement and Evaluation Methods> [Molar Ratio of Styrene / Divinylbenzene / Acenaphthylene] The products and compositions obtained in Examples 1 to 9, 11 to 13 and Comparative Examples 1, 4 to 6 and 9 were dissolved in deuterated chloroform and analyzed by a nuclear magnetic resonance spectrometer (manufactured by JEOL). 1 H-NMR measurement was carried out to determine the molar ratios of repeating units corresponding to styrene, repeating units corresponding to divinylbenzene, and repeating units corresponding to acenaphthylene, and the content of repeating units corresponding to styrene (styrene ratio), the content of repeating units corresponding to divinylbenzene (divinylbenzene ratio), and the content of repeating units corresponding to acenaphthylene (acenaphthylene ratio), relative to 100 mol% of all repeating units, were calculated.

[0061] [Molar ratio of styrene / divinylbenzene / acenaphthylene / vinylcyclohexane] The products obtained in Example 10, Comparative Examples 2 and 7 were dissolved in deuterated chloroform and analyzed by a nuclear magnetic resonance spectrometer (manufactured by JEOL). 1H-NMR measurement was carried out to determine the molar ratios of repeating units corresponding to styrene, repeating units corresponding to divinylbenzene, repeating units relative to acenaphthylene, and repeating units corresponding to vinylcyclohexane, and the content of repeating units corresponding to styrene relative to 100 mol% of all repeating units (styrene ratio), the content of repeating units corresponding to divinylbenzene (divinylbenzene ratio), the content of repeating units corresponding to acenaphthylene (acenaphthylene ratio), and the content of repeating units corresponding to vinylcyclohexane (vinylcyclohexane ratio) were calculated.

[0062] [Molar ratio of styrene / divinylbenzene / isobornyl acrylate] The products obtained in Comparative Examples 3 and 8 were dissolved in deuterated chloroform and analyzed by a nuclear magnetic resonance spectrometer (manufactured by JEOL). 1 H-NMR measurement was carried out to determine the molar ratios of repeating units corresponding to styrene, repeating units corresponding to divinylbenzene, and repeating units corresponding to isobornyl acrylate, and the content of repeating units corresponding to styrene (styrene ratio), the content of repeating units corresponding to divinylbenzene (divinylbenzene ratio), and the content of repeating units corresponding to isobornyl acrylate (isobornyl acrylate ratio) relative to 100 mol% of all repeating units were calculated.

[0063] [Weight-Average Molecular Weight] The products and compositions obtained in Examples 1 to 13 and Comparative Examples 1 to 9 were dissolved in tetrahydrofuran, and the polystyrene-equivalent weight-average molecular weight Mw was measured using gel permeation chromatography (GPC) (Prominence, manufactured by Shimadzu Corporation) connected to four columns (Shodex GPC columns KF-601, KF-602, KF-603, and KF-604, manufactured by Showa Denko) filled with polystyrene gel. A differential refractive index detector (Shodex RI-504, manufactured by Showa Denko) was used, with a column oven temperature of 40°C, a THF flow rate of 0.6 mL / min, a sample concentration of 0.1% by mass, and a sample injection volume of 10 μL.

[0064] [Dielectric Constant, Dielectric Loss Tangent] The products and compositions obtained in Examples 1 to 13 and Comparative Examples 1 to 9 were used as samples. Using a single-action compression molding machine (manufactured by Yasuda Seiki Seisakusho), 1.5 g of sample was pressed at a pressure of 10 MPa and a temperature of 220°C for 15 minutes to prepare a flat plate measuring 30 mm x 30 mm x 1 mm in thickness. The obtained flat plate was cut to prepare test pieces measuring 2 mm in width, 1 mm in thickness, and 30 mm in length. The dielectric constant and dielectric loss tangent of the test pieces at 10 GHz were measured using a cavity resonator dielectric constant measuring device (manufactured by KEYSIGHT), and the results were evaluated according to the following criteria.

[0065] Those with a dielectric constant of less than 2.4 were rated "A" (excellent), those with a dielectric constant of 2.4 or more but less than 2.5 were rated "B" (good), those with a dielectric constant of 2.5 or more but less than 2.6 were rated "C" (fair), those with a dielectric constant of 2.6 or more but less than 2.7 were rated "D" (poor), and those with a dielectric constant of 2.7 or more were rated "E" (poor).

[0066] Those with a dielectric dissipation factor of less than 0.001 were rated as "A" (excellent), those with a dielectric dissipation factor of 0.001 or more and less than 0.002 as "B" (good), those with a dielectric dissipation factor of 0.002 or more and less than 0.003 as "C" (fair), those with a dielectric dissipation factor of 0.003 or more and less than 0.004 as "D" (poor), and those with a dielectric dissipation factor of 0.004 or more as "E" (poor).

[0067] [Glass Transition Temperature Tg] The flat plates prepared according to the above [Dielectric Constant, Dielectric Loss Tangent] were cut to prepare test specimens with a width of 5 mm, a thickness of 1 mm, and a length of 25 mm. The glass transition temperature of these test specimens was measured using a dynamic viscoelasticity measuring device: Rheogel-E4000 (manufactured by UBM Corporation). The maximum value of the loss tangent (tan δ) measured for the test specimens under the conditions of a tensile sine wave, a dynamic strain of 5 μm, a frequency of 1 Hz, and a heating rate of 3 ° C / min was determined as the glass transition temperature. Glass transition temperatures of 180 ° C or higher were rated "A" (excellent), those of 170 ° C or higher but less than 180 ° C were rated "B" (good), those of 160 ° C or higher but less than 170 ° C were rated "C" (fair), and those of less than 160 ° C were rated "D" (poor).

[0068] [Melt Viscosity (Minimum Melt Viscosity)] The products and compositions obtained in Examples 1 to 13 and Comparative Examples 1 to 9 were used as samples. 0.4 g of sample was pressed for 1 minute at a pressure of 10 MPa using a manual hydraulic pump: P-1B (manufactured by Riken) to produce pellets with a diameter of 20 mm and a thickness of 1 mm. Using the obtained pellets as samples, a rheometer: MCR 302 (manufactured by Anton Paar) was used to raise the temperature from 50°C to 200°C at a heating rate of 5°C / min. The minimum value of the complex viscosity was defined as the minimum melt viscosity, and a minimum melt viscosity of less than 100,000 poise was rated as "○" (low viscosity), and a minimum melt viscosity of 100,000 poise or more was rated as "×" (high viscosity).

[0069] (Synthesis Example 1) Synthesis of Compound 1: Vinylbenzyltriphenylphosphonium Chloride 1.5 moles (228.9 g) of vinylbenzyl chloride (trade name: CMS-14, manufactured by AGC Seimi Chemical Co., Ltd.), 1.8 moles (472.1 g) of triphenylphosphine, and 622.4 g of dimethylformamide were placed in a 2.0 L reactor and reacted at 70°C for 3 hours under nitrogen conditions, whereby a white solid precipitated. The solid was thoroughly washed with acetone and then dried under reduced pressure at 92°C, and 490 g of Compound 1 was recovered.

[0070] Synthesis Example 2 Synthesis of Copolymer A 15.1 g of styrene, 13.2 g of Compound 1, 5.5 g of acenaphthylene, 3.5 g of 2,4-diphenyl-4-methyl-1-pentene as a chain transfer agent, 1.28 g of 2,2′-azobis(2,4,4-trimethylpentane) (trade name: VR-110, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) as a polymerization initiator, and 78.8 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120° C. for 3 hours under nitrogen conditions, thereby obtaining Copolymer A as a dimethylformamide solution.

[0071] Synthesis Example 3 Synthesis of Copolymer B 12.7 g of styrene, 16.0 g of Compound 1, 5.0 g of acenaphthylene, 3.5 g of 2,4-diphenyl-4-methyl-1-pentene, 1.28 g of 2,2′-azobis(2,4,4-trimethylpentane), and 78.7 g of dimethylformamide were placed in a 500 mL reactor and reacted at 120° C. for 3 hours under nitrogen conditions, thereby obtaining Copolymer B as a dimethylformamide solution.

[0072] Synthesis Example 4 Synthesis of Copolymer C 18.5 g of styrene, 10.1 g of Compound 1, 6.3 g of acenaphthylene, 3.6 g of 2,4-diphenyl-4-methyl-1-pentene, 1.33 g of 2,2′-azobis(2,4,4-trimethylpentane), and 81.5 g of dimethylformamide were placed in a 500 mL reactor and reacted at 120° C. for 3 hours under nitrogen conditions, to obtain Copolymer C as a dimethylformamide solution.

[0073] Synthesis Example 5 Synthesis of Copolymer D 17.3 g of styrene, 13.5 g of Compound 1, 2.8 g of acenaphthylene, 3.5 g of 2,4-diphenyl-4-methyl-1-pentene, 1.27 g of 2,2′-azobis(2,4,4-trimethylpentane), and 78.2 g of dimethylformamide were placed in a 500 mL reactor and reacted at 120° C. for 3 hours under nitrogen conditions, to obtain Copolymer D as a dimethylformamide solution.

[0074] Synthesis Example 6 Synthesis of Copolymer E 12.8 g of styrene, 12.8 g of Compound 1, 8.0 g of acenaphthylene, 3.5 g of 2,4-diphenyl-4-methyl-1-pentene, 1.28 g of 2,2′-azobis(2,4,4-trimethylpentane), and 78.4 g of dimethylformamide were placed in a 500 mL reactor and reacted at 120° C. for 3 hours under nitrogen conditions, to obtain Copolymer E as a dimethylformamide solution.

[0075] Synthesis Example 7 Synthesis of Copolymer F 17.7 g of styrene, 10.3 g of Compound 1, 8.0 g of acenaphthylene, 3.7 g of 2,4-diphenyl-4-methyl-1-pentene, 1.37 g of 2,2′-azobis(2,4,4-trimethylpentane), and 83.9 g of dimethylformamide were placed in a 500 mL reactor and reacted at 120° C. for 3 hours under nitrogen conditions, to obtain Copolymer F as a dimethylformamide solution.

[0076] Synthesis Example 8 Synthesis of Copolymer G 13.4 g of styrene, 15.8 g of Compound 1, 3.7 g of acenaphthylene, 3.4 g of 2,4-diphenyl-4-methyl-1-pentene, 1.25 g of 2,2′-azobis(2,4,4-trimethylpentane), and 76.7 g of dimethylformamide were placed in a 500 mL reactor and reacted at 120° C. for 3 hours under nitrogen conditions, to obtain Copolymer G as a dimethylformamide solution.

[0077] Synthesis Example 9 Synthesis of Copolymer H 10.2 g of styrene, 15.0 g of Compound 1, 7.0 g of acenaphthylene, 3.4 g of 2,4-diphenyl-4-methyl-1-pentene, 1.22 g of 2,2′-azobis(2,4,4-trimethylpentane), and 75.2 g of dimethylformamide were placed in a 500 mL reactor and reacted at 120° C. for 3 hours under nitrogen conditions, thereby obtaining Copolymer H as a dimethylformamide solution.

[0078] Synthesis Example 10 Synthesis of Copolymer I 21.7 g of styrene, 10.6 g of Compound 1, 3.3 g of acenaphthylene, 3.7 g of 2,4-diphenyl-4-methyl-1-pentene, 1.35 g of 2,2′-azobis(2,4,4-trimethylpentane), and 82.9 g of dimethylformamide were placed in a 500 mL reactor and reacted at 120° C. for 3 hours under nitrogen conditions, thereby obtaining Copolymer I as a dimethylformamide solution.

[0079] Synthesis Example 11 Synthesis of Copolymer J 9.7 g of styrene, 12.0 g of Compound 1, 5.0 g of acenaphthylene, 8.5 g of vinylcyclohexane, 3.8 g of 2,4-diphenyl-4-methyl-1-pentene, 1.34 g of 2,2′-azobis(2,4,4-trimethylpentane), and 82.2 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120° C. for 3 hours under nitrogen conditions, thereby obtaining Copolymer J as a dimethylformamide solution.

[0080] Synthesis Example 12 Synthesis of Copolymer K 18.5 g of styrene, 10.1 g of Compound 1, 6.3 g of acenaphthylene, 3.7 g of 2,4-diphenyl-4-methyl-1-pentene, 0.77 g of di-tert-butyl peroxide (trade name: Perbutyl D, manufactured by NOF Corp.) as a polymerization initiator, and 81.5 g of dimethylformamide were charged into a 500 mL reactor and reacted at 132° C. for 3 hours under nitrogen conditions, thereby obtaining Copolymer K as a dimethylformamide solution.

[0081] Synthesis Example 13 Synthesis of Copolymer L 15.1 g of styrene, 13.2 g of Compound 1, 5.5 g of acenaphthylene, 1.8 g of 2,4-diphenyl-4-methyl-1-pentene, 1.28 g of 2,2′-azobis(2,4,4-trimethylpentane), and 78.8 g of dimethylformamide were placed in a 500 mL reactor and reacted at 120° C. for 3.5 hours under nitrogen conditions, to obtain Copolymer L as a dimethylformamide solution.

[0082] Synthesis Example 14 Synthesis of Copolymer M 18.5 g of styrene, 10.1 g of Compound 1, 6.3 g of acenaphthylene, 7.3 g of 2,4-diphenyl-4-methyl-1-pentene, 2.65 g of 2,2′-azobis(2,4,4-trimethylpentane), and 81.5 g of dimethylformamide were placed in a 500 mL reactor and reacted at 120° C. for 1.5 hours under nitrogen conditions, to obtain Copolymer M as a dimethylformamide solution.

[0083] Comparative Synthesis Example 1 Synthesis of Copolymer N 22.0 g of styrene, 15.5 g of Compound 1, 3.9 g of 2,4-diphenyl-4-methyl-1-pentene, 0.82 g of di-tert-butyl peroxide, and 87.4 g of dimethylformamide were placed in a 500 mL reactor and reacted at 132°C for 3 hours under nitrogen conditions to obtain Copolymer N as a dimethylformamide solution.

[0084] Comparative Synthesis Example 2 Synthesis of Copolymer O 14.3 g of styrene, 12.4 g of Compound 1, 8.0 g of vinylcyclohexane, 3.7 g of 2,4-diphenyl-4-methyl-1-pentene, 0.76 g of di-tert-butyl peroxide, and 81.0 g of dimethylformamide were placed in a 500 mL reactor and reacted at 132°C for 3 hours under nitrogen conditions, to obtain Copolymer O as a dimethylformamide solution.

[0085] Comparative Synthesis Example 3 Synthesis of Copolymer P 14.1 g of styrene, 11.4 g of Compound 1, 8.0 g of isobornyl acrylate, 3.5 g of 2,4-diphenyl-4-methyl-1-pentene, 0.74 g of di-tert-butyl peroxide, and 78.3 g of dimethylformamide were placed in a 500 mL reactor and reacted at 132°C for 3 hours under nitrogen conditions, to obtain Copolymer P as a dimethylformamide solution.

[0086] Comparative Synthesis Example 4 Synthesis of Copolymer Q 22.0 g of styrene, 15.5 g of Compound 1, 3.9 g of 2,4-diphenyl-4-methyl-1-pentene, 1.42 g of 2,2′-azobis(2,4,4-trimethylpentane), and 87.4 g of dimethylformamide were placed in a 500 mL reactor and reacted at 120° C. for 2 hours under nitrogen conditions, to obtain Copolymer Q as a dimethylformamide solution.

[0087] Comparative Synthesis Example 5 Synthesis of Copolymer R 10.6 g of Compound 1, 22.0 g of acenaphthylene, 3.4 g of 2,4-diphenyl-4-methyl-1-pentene, 1.24 g of 2,2′-azobis(2,4,4-trimethylpentane), and 76.0 g of dimethylformamide were placed in a 500 mL reactor and reacted at 120° C. for 3 hours under nitrogen conditions, to obtain Copolymer R as a dimethylformamide solution.

[0088] Comparative Synthesis Example 6 Synthesis of Copolymer S 14.3 g of styrene, 12.4 g of Compound 1, 8.0 g of vinylcyclohexane, 3.6 g of 2,4-diphenyl-4-methyl-1-pentene, 1.32 g of 2,2′-azobis(2,4,4-trimethylpentane), and 81.0 g of dimethylformamide were placed in a 500 mL reactor and reacted at 120° C. for 3 hours under nitrogen conditions, to obtain Copolymer S as a dimethylformamide solution.

[0089] Comparative Synthesis Example 7 Synthesis of Copolymer T 14.1 g of styrene, 11.4 g of Compound 1, 8.0 g of isobornyl acrylate, 3.5 g of 2,4-diphenyl-4-methyl-1-pentene, 1.27 g of 2,2′-azobis(2,4,4-trimethylpentane), and 78.3 g of dimethylformamide were placed in a 500 mL reactor and reacted at 120° C. for 3 hours under nitrogen conditions, to obtain Copolymer T as a dimethylformamide solution.

[0090] Comparative Synthesis Example 8 Synthesis of Polymer U 35.0 g of acenaphthylene, 3.6 g of 2,4-diphenyl-4-methyl-1-pentene, 1.33 g of 2,2'-azobis(2,4,4-trimethylpentane), and 81.7 g of dimethylformamide were placed in a 500 mL reactor and reacted at 120°C for 4 hours under nitrogen conditions. This reaction solution was reprecipitated in a large excess of methanol, and the supernatant was decanted. The remaining solid was dried under reduced pressure at 92°C, and 33.9 g of Polymer U was recovered.

[0091] Example 1: 117.4 g of a dimethylformamide solution of copolymer A obtained in Synthesis Example 2, 117.4 g of toluene, 31.1 g of 37% by weight formalin, and 38.3 g of a 28% by weight aqueous potassium hydroxide solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. The organic layer was dehydrated and concentrated, and then 18.2 g of anhydrous magnesium chloride was added and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. The solid was then filtered off and dried under reduced pressure at 60°C to recover 14.2 g of product 1. The Mw of product 1 was 5500, the styrene ratio was 62.1 mol%, the divinylbenzene ratio was 16.2 mol%, and the acenaphthylene ratio was 21.7 mol%.

[0092] Example 2: 117.2 g of a dimethylformamide solution of copolymer B obtained in Synthesis Example 3, 117.2 g of toluene, 37.6 g of 37% by mass formalin, and 46.5 g of a 28% by mass aqueous potassium hydroxide solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 22.1 g of anhydrous magnesium chloride was added and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. The solid was then filtered and dried under reduced pressure at 60°C to recover 13.0 g of product 2. The Mw of product 2 was 5400, the styrene ratio was 57.9 mol%, the divinylbenzene ratio was 20.8 mol%, and the acenaphthylene ratio was 21.3 mol%.

[0093] Example 3: 121.4 g of the dimethylformamide solution of copolymer C obtained in Synthesis Example 4, 121.4 g of toluene, 23.7 g of 37% by mass formalin, and 29.3 g of 28% by mass aqueous potassium hydroxide solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. The organic layer was dehydrated and concentrated, and then 13.9 g of anhydrous magnesium chloride was added and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. The solid was then filtered and dried under reduced pressure at 60°C to recover 16.4 g of product 3. The Mw of product 3 was 5500, the styrene ratio was 66.9 mol%, the divinylbenzene ratio was 10.4 mol%, and the acenaphthylene ratio was 22.7 mol%.

[0094] Example 4: 116.5 g of a dimethylformamide solution of copolymer D obtained in Synthesis Example 5, 116.5 g of toluene, 31.6 g of 37% by mass formalin, and 39.0 g of a 28% by mass aqueous potassium hydroxide solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After dehydration and concentration of the organic layer, 18.6 g of anhydrous magnesium chloride was added and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. The solid was then filtered and dried under reduced pressure at 60°C to recover 14.0 g of product 4. The Mw of product 4 was 5700, the styrene ratio was 73.5 mol%, the divinylbenzene ratio was 17.0 mol%, and the acenaphthylene ratio was 9.5 mol%.

[0095] Example 5: 116.8 g of a dimethylformamide solution of copolymer E obtained in Synthesis Example 6, 116.8 g of toluene, 30.1 g of 37% by mass formalin, and 37.2 g of a 28% by mass aqueous potassium hydroxide solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. The organic layer was dehydrated and concentrated, and then 17.7 g of anhydrous magnesium chloride was added and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. The solid was then filtered off and dried under reduced pressure at 60°C to recover 14.6 g of product 5. The Mw of product 5 was 5100, the styrene ratio was 52.3 mol%, the divinylbenzene ratio was 15.7 mol%, and the acenaphthylene ratio was 32.0 mol%.

[0096] Example 6: 125.0 g of a dimethylformamide solution of copolymer F obtained in Synthesis Example 7, 125.0 g of toluene, 24.1 g of 37% by mass formalin, and 29.7 g of a 28% by mass aqueous potassium hydroxide solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. The organic layer was dehydrated and concentrated, and then 14.1 g of anhydrous magnesium chloride was added and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. The solid was then filtered off and dried under reduced pressure at 60°C to recover 16.9 g of product 6. The Mw of product 6 was 5200, the styrene ratio was 63.0 mol%, the divinylbenzene ratio was 10.6 mol%, and the acenaphthylene ratio was 26.4 mol%.

[0097] Example 7: 114.3 g of a dimethylformamide solution of copolymer G obtained in Synthesis Example 8, 114.3 g of toluene, 37.1 g of 37% by mass formalin, and 45.9 g of a 28% by mass aqueous potassium hydroxide solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. The organic layer was dehydrated and concentrated, and then 21.8 g of anhydrous magnesium chloride was added and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. The solid was then filtered off and dried under reduced pressure at 60°C to recover 12.7 g of product 7. Product 7 had an Mw of 5700, a styrene ratio of 63.5 mol%, a divinylbenzene ratio of 20.8 mol%, and an acenaphthylene ratio of 15.7 mol%.

[0098] Example 8: 111.9 g of a dimethylformamide solution of copolymer H obtained in Synthesis Example 9, 111.9 g of toluene, 35.1 g of 37% by mass formalin, and 43.4 g of a 28% by mass aqueous potassium hydroxide solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. The organic layer was dehydrated and concentrated, and then 20.6 g of anhydrous magnesium chloride was added and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. The solid was then removed by filtration and dried under reduced pressure at 60°C to recover 12.9 g of product 8. The Mw of product 8 was 6000, the styrene ratio was 49.1 mol%, the divinylbenzene ratio was 20.2 mol%, and the acenaphthylene ratio was 30.7 mol%.

[0099] Example 9: 123.5 g of a dimethylformamide solution of copolymer I obtained in Synthesis Example 10, 123.5 g of toluene, 24.9 g of 37% by weight formalin, and 30.7 g of a 28% by weight aqueous potassium hydroxide solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. The organic layer was dehydrated and concentrated, and then 14.6 g of anhydrous magnesium chloride was added and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. The solid was then filtered and dried under reduced pressure at 60°C to recover 16.6 g of product 9. The Mw of product 9 was 5100, the styrene ratio was 79.0 mol%, the divinylbenzene ratio was 9.7 mol%, and the acenaphthylene ratio was 11.3 mol%.

[0100] Example 10: 122.5 g of a dimethylformamide solution of copolymer J obtained in Synthesis Example 11, 122.5 g of toluene, 28.2 g of 37% by weight formalin, and 34.9 g of a 28% by weight aqueous potassium hydroxide solution were placed in a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 16.6 g of anhydrous magnesium chloride was added and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. The solid was then removed by filtration and dried under reduced pressure at 60°C to recover 15.7 g of product 10. The Mw of product 10 was 6400, the styrene ratio was 42.9 mol%, the divinylbenzene ratio was 16.8 mol%, the acenaphthylene ratio was 21.9 mol%, and the vinylcyclohexane ratio was 18.4 mol%.

[0101] Example 11: 120.8 g of a dimethylformamide solution of copolymer K obtained in Synthesis Example 12, 120.8 g of toluene, 23.7 g of 37% by mass formalin, and 29.3 g of a 28% by mass aqueous potassium hydroxide solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. The organic layer was dehydrated and concentrated, and then 13.9 g of anhydrous magnesium chloride was added and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. The solid was then removed by filtration and dried under reduced pressure at 60°C to recover 16.5 g of product 11. The Mw of product 11 was 5200, the styrene ratio was 62.7 mol%, the divinylbenzene ratio was 16.0 mol%, and the acenaphthylene ratio was 21.3 mol%.

[0102] Example 12: 115.7 g of a dimethylformamide solution of copolymer L obtained in Synthesis Example 13, 115.7 g of toluene, 31.1 g of 37% by mass formalin, and 38.3 g of a 28% by mass aqueous potassium hydroxide solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. The organic layer was dehydrated and concentrated, and then 18.2 g of anhydrous magnesium chloride was added and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. The solid was then filtered off and dried under reduced pressure at 60°C to recover 14.3 g of product 12. The Mw of product 12 was 10900, the styrene ratio was 60.7 mol%, the divinylbenzene ratio was 16.9 mol%, and the acenaphthylene ratio was 22.4 mol%.

[0103] Example 13: 126.3 g of a dimethylformamide solution of copolymer M obtained in Synthesis Example 14, 126.3 g of toluene, 23.7 g of 37% by mass formalin, and 29.3 g of a 28% by mass aqueous potassium hydroxide solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. The organic layer was dehydrated and concentrated, and then 13.9 g of anhydrous magnesium chloride was added and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. The solid was then removed by filtration and dried under reduced pressure at 60°C to recover 16.5 g of product 13. The Mw of product 13 was 2600, the styrene ratio was 64.7 mol%, the divinylbenzene ratio was 15.0 mol%, and the acenaphthylene ratio was 20.3 mol%.

[0104] Comparative Example 1 129.7 g of a dimethylformamide solution of copolymer N obtained in Comparative Synthesis Example 1, 129.7 g of toluene, 36.2 g of 37% by weight formalin, and 44.7 g of a 28% by weight aqueous potassium hydroxide solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. The organic layer was dehydrated and concentrated, and then 21.3 g of anhydrous magnesium chloride was added and stirred at 65 ° C. for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. The solid was then removed by filtration, and 15.6 g of product 14 was recovered by drying under reduced pressure at 60 ° C. The Mw of product 14 was 5600, the styrene ratio was 83.2 mol%, and the divinylbenzene ratio was 16.8 mol%.

[0105] Comparative Example 2: 120.1 g of a dimethylformamide solution of copolymer O obtained in Comparative Synthesis Example 2, 120.1 g of toluene, 29.1 g of 37% by weight formalin, and 35.9 g of a 28% by weight aqueous potassium hydroxide solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. The organic layer was dehydrated and concentrated, and then 17.1 g of anhydrous magnesium chloride was added and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. The solid was then removed by filtration and dried under reduced pressure at 60°C to recover 15.2 g of product 15. The Mw of product 15 was 6000, the styrene ratio was 63.9 mol%, the divinylbenzene ratio was 15.8 mol%, and the vinylcyclohexane ratio was 20.3 mol%.

[0106] Comparative Example 3: 116.1 g of a dimethylformamide solution of copolymer P obtained in Comparative Synthesis Example 3, 116.1 g of toluene, 26.9 g of 37% by weight formalin, and 33.1 g of a 28% by weight aqueous potassium hydroxide solution were added to a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. The organic layer was dehydrated and concentrated, and then 15.8 g of anhydrous magnesium chloride was added and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. The solid was then removed by filtration and dried under reduced pressure at 60°C to recover 14.9 g of product 16. The Mw of product 16 was 5500, the styrene ratio was 63.2 mol%, the divinylbenzene ratio was 15.7 mol%, and the isobornyl acrylate ratio was 21.1 mol%.

[0107] Comparative Example 4: 130.2 g of a dimethylformamide solution of copolymer Q obtained in Comparative Synthesis Example 4, 130.2 g of toluene, 36.3 g of 37% by weight formalin, and 44.9 g of a 28% by weight aqueous potassium hydroxide solution were added to a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. The organic layer was dehydrated and concentrated, and then 21.3 g of anhydrous magnesium chloride was added and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. The solid was then removed by filtration and dried under reduced pressure at 60°C to recover 15.7 g of product 17. The Mw of product 17 was 6200, the styrene ratio was 84.4 mol%, and the divinylbenzene ratio was 15.6 mol%.

[0108] Comparative Example 5: 77.6 g of styrene, 20.0 g of acenaphthylene, 10.2 g of 2,4-diphenyl-4-methyl-1-pentene, 3.71 g of 2,2'-azobis(2,4,4-trimethylpentane), and 227.6 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 3 hours under nitrogen. This reaction solution was reprecipitated in a large excess of methanol, and the supernatant was decanted. The remaining solid was dried under reduced pressure at 80°C, and 58.2 g of product 18 was recovered. The Mw of product 18 was 4900, the styrene ratio was 76.9 mol%, and the acenaphthylene ratio was 23.1 mol%.

[0109] Comparative Example 6: 113.2 g of a dimethylformamide solution of copolymer R obtained in Comparative Synthesis Example 5, 113.2 g of toluene, 24.9 g of 37% by weight formalin, and 30.7 g of a 28% by weight aqueous potassium hydroxide solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. The organic layer was dehydrated and concentrated, and then 14.6 g of anhydrous magnesium chloride was added and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. The solid was then filtered off and dried under reduced pressure at 60°C to recover 14.9 g of product 19. Product 19 had an Mw of 4700, a divinylbenzene ratio of 13.0 mol%, and an acenaphthylene ratio of 87.0 mol%.

[0110] Comparative Example 7: 120.6 g of a dimethylformamide solution of copolymer S obtained in Comparative Synthesis Example 6, 120.6 g of toluene, 29.1 g of 37% by weight formalin, and 35.9 g of a 28% by weight aqueous potassium hydroxide solution were added to a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. The organic layer was dehydrated and concentrated, and then 17.1 g of anhydrous magnesium chloride was added and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. The solid was then removed by filtration and dried under reduced pressure at 60°C to recover 15.2 g of product 20. The Mw of product 20 was 6300, the styrene ratio was 62.1 mol%, the divinylbenzene ratio was 16.5 mol%, and the vinylcyclohexane ratio was 21.4 mol%.

[0111] Comparative Example 8: 116.6 g of a dimethylformamide solution of copolymer T obtained in Comparative Synthesis Example 7, 116.6 g of toluene, 26.9 g of 37% by weight formalin, and 33.1 g of a 28% by weight aqueous potassium hydroxide solution were added to a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. The organic layer was dehydrated and concentrated, and then 15.8 g of anhydrous magnesium chloride was added and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. The solids were then removed by filtration and dried under reduced pressure at 60°C to recover 15.0 g of product 21. The Mw of product 21 was 5700, the styrene ratio was 63.8 mol%, the divinylbenzene ratio was 15.5 mol%, and the isobornyl acrylate ratio was 20.7 mol%.

[0112] Comparative Example 9 5.7 g of Product 17 obtained in Comparative Example 4 and 2.0 g of Polymer U obtained in Comparative Synthesis Example 8 were mixed and dissolved in toluene to form a homogeneous solution. This solution was dried under reduced pressure at 60°C to recover 7.3 g of Composition 1. Composition 1 had an Mw of 6100, a styrene ratio of 67.5 mol%, a divinylbenzene ratio of 12.5 mol%, and an acenaphthylene ratio of 20.0 mol%.

[0113] The dielectric constant, dielectric loss tangent, glass transition temperature, and melt viscosity were evaluated for the products and compositions obtained in Examples 1 to 13 and Comparative Examples 1 to 9. The results are shown in Tables 1 to 5 below.

[0114]

[0115]

[0116]

[0117]

[0118]

[0119] Example 11 and Comparative Examples 1 to 3 are examples in which a peroxide-type polymerization initiator was used. In Comparative Example 1, the glass transition temperature was poor due to the absence of acenaphthylene units. In Comparative Example 2, vinylcyclohexane was added as a monomer to Comparative Example 1 for copolymerization, but the glass transition temperature did not improve. In Comparative Example 3, isobornyl acrylate was added as a monomer to Comparative Example 1 for copolymerization, and although the glass transition temperature was improved, both the dielectric constant and the dielectric loss tangent deteriorated due to the presence of ester groups.

[0120] In contrast to this, in Example 11, by incorporating an acenaphthylene unit compared to Comparative Example 1, the dielectric constant and dielectric loss tangent were somewhat improved, and the glass transition temperature was significantly improved, thereby achieving both dielectric properties and glass transition temperature. In Example 11, the minimum melt viscosity was also low.

[0121] Examples 1 to 10, 12 to 13 and Comparative Examples 4 to 9 are examples in which the azo-based initiator of the above formula (1) was used. In Comparative Example 4, the dielectric properties were improved compared to Comparative Example 1, but due to the absence of an acenaphthylene unit, the glass transition temperature was inferior, similar to Comparative Example 1.

[0122] In Comparative Example 5, the divinylbenzene unit was not present, and thermal curing did not proceed. Therefore, test pieces for evaluating the dielectric constant, dielectric loss tangent, and glass transition temperature could not be prepared, and these items could not be evaluated. Furthermore, since thermal curing did not proceed, the melt viscosity continued to decrease monotonically, and the minimum melt viscosity could not be observed.

[0123] In Comparative Example 6, the dielectric properties and glass transition temperature were excellent, but the absence of styrene units resulted in a high minimum melt viscosity and poor processability. In Comparative Example 7, vinylcyclohexane was added as a monomer to Comparative Example 4 for copolymerization, but the glass transition temperature did not improve. In Comparative Example 8, isobornyl acrylate was added as a monomer to Comparative Example 4 for copolymerization, and although the glass transition temperature was improved, both the dielectric constant and dielectric loss tangent deteriorated due to the presence of ester groups.

[0124] In Comparative Example 9, Product 17 of Comparative Example 4 was mixed with Polymer U, which was a homopolymer of acenaphthylene, and the composition contained styrene units, divinylbenzene units, and acenaphthylene units. However, the glass transition temperature was poor, the minimum melt viscosity was high, and the processability was poor.

[0125] In contrast, in Examples 1 to 10 and 12 to 13, by incorporating an acenaphthylene unit compared to Comparative Example 4, excellent dielectric constant and dielectric loss tangent were generally maintained while the glass transition temperature was excellent, and both the dielectric properties and the glass transition temperature were achieved. In addition, the minimum melt viscosity was low.

[0126] Furthermore, the products of Examples 1 to 13 were excellent in formability, being able to be molded into sheets sufficient to stand on their own without the use of a thermoplastic resin or a crosslinking agent.

[0127] The various numerical ranges described in this specification can be arbitrarily combined with their respective upper and lower limit values, and all such combinations are considered to be preferred numerical ranges described in this specification. Furthermore, a numerical range described as "X to Y" means from X to Y.

[0128] Although several embodiments of the present invention have been described above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their omissions, substitutions, modifications, etc. are included within the scope and spirit of the invention, as well as within the scope of the invention described in the claims and their equivalents.

Claims

1. A thermosetting resin which is a linear copolymer having a repeating unit corresponding to a monovinyl aromatic compound, a repeating unit corresponding to a divinyl aromatic compound, and a repeating unit corresponding to an aromatic ring-fused cyclic olefin compound.

2. The thermosetting resin according to claim 1, wherein the content of the repeating units corresponding to the aromatic ring-fused cyclic olefin compound is 5 to 80 mol % in 100 mol % of all repeating units.

3. A straight-chain copolymer having a terminal end having the general formula (1): R 1 -N=N-R 2 In the general formula (1), R 1 and R 2 The thermosetting resin according to claim 1 , wherein each independently represents a monovalent saturated hydrocarbon group or a monovalent aromatic hydrocarbon group.

4. The thermosetting resin according to claim 1, wherein the total content of the repeating units corresponding to the monovinyl aromatic compound, the repeating units corresponding to the divinyl aromatic compound, and the repeating units corresponding to the aromatic ring-fused cyclic olefin compound is 80 mol % or more, based on 100 mol % of all repeating units.

5. The thermosetting resin according to claim 1, wherein the number of rings in the aromatic ring-fused cyclic olefin compound is 3 or less.

6. A cured product obtained by curing the thermosetting resin according to any one of claims 1 to 5.

7. A thermosetting composition comprising the thermosetting resin according to any one of claims 1 to 5.

8. The thermosetting composition according to claim 7, which is a printed circuit board material.

Citation Information

Patent Citations

  • Thermosetting resin composition, its cured item, and circuit board including the cured item

    JP2001192539A

  • Curable resin composition

    JP2004131638A

  • Curable resin composition

    JP2006274169A

  • Curable resin composition, cured product and optical article

    JP2013133375A

  • Thermosetting resins and their cured products

    JP7017662B1

Cited By

  • Resin composition, prepreg and application of prepreg in rigid-flex printed circuit board

    CN121517885A

  • Resin composition, prepreg, film with resin, metal foil with resin, metal-clad laminate, and wiring board