Lithium-ion battery
The lithium ion battery design with a silver-based negative electrode current collector and high lithium aluminate content separator ensures reliable operation at high temperatures by preventing short circuits and maintaining charging characteristics, addressing the degradation issues in existing lithium ion batteries.
Patent Information
- Application Number
- PCT/JP2024/011333
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-03
AI Technical Summary
Lithium ion batteries face degradation of charging characteristics in high-temperature environments, leading to reliability issues.
A lithium ion battery design featuring an integral sintered body with multiple positive and negative electrode layers and a ceramic separator, where the negative electrode current collector layer contains silver and the separator is predominantly lithium aluminate (LiAlO2) with a content ratio of 50% or more by volume, enhancing reliability and preventing short circuits at high temperatures.
The battery maintains stable charging characteristics even at high temperatures (above 80°C) with improved reliability and capacity, as the silver-based current collector and lithium aluminate separator configuration effectively prevent short circuits and enhance lithium ion conductivity.
Smart Images

Figure JP2024011333_03102024_PF_FP_ABST
Abstract
Description
Lithium-ion battery
[0001] This disclosure relates to a lithium-ion battery. This application claims priority to Japanese Patent Application No. 2023-058368, filed on March 31, 2023, and incorporates by reference all of the contents of said Japanese Patent Application.
[0002] A known lithium-ion battery includes a positive electrode layer made of a sintered body of a lithium composite oxide, a negative electrode layer made of a sintered body containing titanium, and a ceramic separator disposed between the positive electrode layer and the negative electrode layer. Patent Document 1 (WO 2019 / 221140) discloses a lithium-ion battery that includes a positive electrode layer, a ceramic separator, and a negative electrode layer bonded to each other as an integral sintered plate, and is impregnated with an electrolyte. The lithium-ion battery disclosed in Patent Document 1 includes a ceramic separator made of MgO and glass as the separator.
[0003] Patent Document 2 discloses an all-solid-state battery having a laminate in which multiple positive electrode layers and multiple negative electrode layers are alternately stacked with solid electrolyte layers interposed therebetween. In the examples of Patent Document 2 (JP 2021-027044 A), a laminate is disclosed in which lithium vanadium phosphate is used as the positive electrode active material layer and the negative electrode active material layer, and lithium aluminum titanium phosphate is used as the solid electrolyte layer. It also discloses the use of copper and lithium vanadium phosphate as the positive electrode current collector layer and the negative electrode current collector layer.
[0004] International Publication No. 2019 / 221140 Japanese Patent Application Laid-Open No. 2021-027044
[0005] The range of applications for lithium-ion batteries continues to expand, and there is a demand for batteries that are highly reliable and do not lose their charging characteristics even when placed in harsher environments, especially high-temperature environments.
[0006] In view of this situation, one of the objects of the invention of the present disclosure is to provide a highly reliable lithium ion battery whose charging characteristics do not deteriorate even when placed in a high-temperature environment.
[0007] A lithium-ion battery according to the present disclosure includes a plurality of positive electrode layers, a plurality of negative electrode layers, and a separator disposed between the positive electrode layers and the negative electrode layers. The lithium-ion battery also includes an electrode including an integrated sintered body in which the positive electrode layers, the negative electrode layers, and the separator are sintered together, an electrolyte impregnated in the electrode, and an exterior housing containing the electrode and the electrolyte. The electrode includes a negative electrode current collector layer in contact with the negative electrode layer. The negative electrode current collector layer contains Ag. The separator is made of LiAlO 2 The separator contains LiAlO 2 The content ratio of is 50% by volume or more.
[0008] According to the lithium ion battery, the charging characteristics do not deteriorate even when placed in a high temperature environment, and a highly reliable lithium ion battery is provided.
[0009] FIG. 1 is a schematic cross-sectional view showing a lithium ion battery according to the present disclosure. FIG. 2 is a schematic cross-sectional perspective view showing a laminated portion included in a lithium ion battery according to the present disclosure. FIG. 3 is a schematic perspective view showing a sintered body included in a lithium ion battery according to the present disclosure. FIG. 4 is a schematic perspective view showing a sintered body included in a lithium ion battery according to the present disclosure. FIG. 5 is a schematic view showing a part of a manufacturing process for a sintered body included in a lithium ion battery according to the present disclosure. FIG. 6 is a schematic view showing a part of a manufacturing process for a sintered body included in a lithium ion battery according to the present disclosure. FIG. 7 is a schematic view showing a part of a manufacturing process for a sintered body included in a lithium ion battery according to the present disclosure. FIG. 8 is a schematic perspective view showing the appearance of a lithium ion battery according to the present disclosure.
[0010] [Summary of the embodiment] First, embodiments of the present disclosure will be listed and described. A lithium ion battery according to the present disclosure includes a plurality of positive electrode layers, a plurality of negative electrode layers, and a separator disposed between the positive electrode layers and the negative electrode layers. The lithium ion battery includes an electrode including an integrated sintered body in which the plurality of positive electrode layers, the plurality of negative electrode layers, and the separator are sintered together, an electrolyte impregnated in the electrode, and an exterior body accommodating the electrode and the electrolyte. The electrode includes a negative electrode current collector layer in contact with the negative electrode layer. The negative electrode current collector layer contains Ag. The separator is made of LiAlO 2 The separator contains LiAlO 2 The content ratio of is 50% by volume or more.
[0011] Conventionally, lithium ion batteries have been known that include a laminate including multiple positive electrode layers and multiple negative electrode layers, with multiple cells configured within one electrode (see, for example, Patent Document 2). Patent Document 2 discloses that a material with excellent conductivity can be used for the positive electrode current collector layer or the negative electrode current collector layer, such as silver, palladium, gold, platinum, aluminum, copper, or nickel. However, in addition to the examples disclosed in Patent Document 2, the negative electrode current collector in lithium ion batteries is exclusively made of a material containing copper.
[0012] Aiming to further improve the performance of lithium-ion batteries, specific configurations for using Ag as the negative electrode current collector layer in electrodes having a multilayer laminate structure, particularly in electrodes that are integrally sintered bodies in which a positive electrode layer, a negative electrode layer, and a separator are sintered together, have been investigated. When a negative electrode current collector layer containing Ag is adopted, a separator made of LiAlO 2 It has been found that lithium ion batteries employing ceramic separators containing LiAlO do not short-circuit even when stored for long periods of time in high-temperature environments of 80°C or higher, and are highly reliable. 2The use of a separator having a novel structure was not anticipated. The electrode for a lithium-ion battery according to the present disclosure uses a separator having a novel structure. By using such an electrode, a highly reliable lithium-ion battery can be provided, in which the charging characteristics are not deteriorated even when the battery is placed in a high-temperature environment.
[0013] In the lithium ion battery, the separator is LiAlO 2 and LiAlO 2 When the separator has this configuration, the effects of the present disclosure can be reliably obtained.
[0014] In the lithium-ion battery, the positive electrode layer may be composed of a lithium composite oxide sintered body, and the negative electrode layer may be composed of a titanium-containing sintered body. Electrodes in which the positive electrode layer and the negative electrode layer are integrally sintered bodies having these structures are known, and can be used to construct high-capacity, highly durable lithium-ion batteries. By combining this with the aforementioned negative electrode current collector and separator, a lithium-ion battery with high capacity and no deterioration in charging characteristics even at high temperatures can be obtained.
[0015] In the lithium ion battery, the thickness of the negative electrode current collector layer may be 0.1 μm or more and 60 μm or less, and the thickness of the separator may be 1 μm or more and 50 μm or less. When the thicknesses of the negative electrode current collector and the separator are within these ranges, a small-sized, high-capacity lithium ion battery can be configured that includes a large number of cells.
[0016] [Specific Examples of Embodiments] Next, specific examples of embodiments of the lithium ion battery of the present disclosure will be described with reference to the drawings. In the following drawings, the same or corresponding parts are designated by the same reference numerals, and their description will not be repeated.
[0017] (Lithium-ion Battery) First, an overview of a lithium-ion battery according to the present disclosure will be described. FIG. 1 is a schematic cross-sectional view showing the structure of a lithium-ion battery 10, which is an example of an embodiment according to the present disclosure. FIG. 2 is a schematic cross-sectional perspective view showing a laminated portion 1 of a sintered body 9 included in the lithium-ion battery 10. FIG. 3 is a schematic perspective view showing a sintered body 9 included in the lithium-ion battery 10. In this specification, the direction along the X-axis shown in FIGS. 1 to 3 is referred to as the width direction of the laminated portion 1 or the sintered body 9, the direction along the Y-axis is referred to as the depth direction of the laminated portion 1 or the sintered body 9, and the direction along the Z-axis is referred to as the stacking direction or thickness direction of the laminated portion 1 or the sintered body 9. In this specification, the surface of the top layer in the stacking direction of the laminated portion 1 is referred to as the top surface, the surface of the bottom layer in the stacking direction is referred to as the bottom surface, and the surfaces on which all the stacked layers are exposed are referred to as the front and back surfaces. The front and back surfaces are surfaces parallel to the XZ plane. Furthermore, in the laminated unit 1, the surface on which the laminated structure is exposed, which extends between the front and back surfaces and along the depth direction, is referred to as the side surface. The side surface is a surface parallel to the YZ plane. Surfaces other than the top and bottom surfaces, that is, the front and back surfaces in addition to the side surfaces, may also be referred to as the side surface. Note that the terms top surface, bottom surface, side surface, etc. are relative terms used for the convenience of explanation in this specification, and it goes without saying that the arrangement direction and use direction of the lithium-ion battery are not limited to these directions.
[0018] Referring to Fig. 1, a lithium-ion battery 10 includes an electrode 5 housed inside an exterior body 24. The electrode 5 includes a sintered body 9, a positive electrode current collector 14, and a negative electrode current collector 18 attached to both side surfaces of the sintered body 9. Referring to Fig. 3, the sintered body 9 includes a laminated portion 1 and an insulating portion 51 serving as an insulating ceramic portion extending around the periphery of the laminated portion 1. Referring to Figs. 1 and 3, the laminated portion 1 is formed by stacking a plurality of positive electrode layers 12, a plurality of negative electrode layers 16, and a separator 20. The laminated portion 1 and the insulating portion 51 together constitute the sintered body 9, which is a single, integrated sintered body.
[0019] In the laminate 1, the positive electrode layers 12 and the negative electrode layers 16 are alternately stacked in the stacking direction (Z-axis direction). A separator 20 is interposed between the positive electrode layers 12 and the negative electrode layers 16. The separator 20 separates the positive electrode layers 12 and the negative electrode layers 16 from each other. The positive electrode layers 12 are made of, for example, a sintered body containing lithium cobalt oxide. The negative electrode layers 16 are made of, for example, a sintered body containing titanium. The separator 20 is made of ceramic.
[0020] 1 , the electrode 5 of the lithium-ion battery 10 includes a positive electrode current collector 14 that is disposed in contact with the sintered body 9 from the side surface to the bottom surface of the sintered body 9. The lithium-ion battery 10 also includes a negative electrode current collector 18 that is disposed in contact with the sintered body 9 from the side surface to the top surface of the sintered body 9. The positive electrode current collector 14 and the negative electrode current collector 18 may be metal foils such as aluminum foils. The positive electrode current collector 14 is made of LiCoO 2 , which is the positive electrode active material that constitutes the positive electrode layer 12. 2 containing LiCoO 2 The negative electrode current collector 18 may be made of copper foil, silver foil, or silver. From the viewpoint of reducing contact resistance, a carbon layer (not shown) is preferably provided between the positive electrode current collector 14 and the negative electrode current collector 18 and the sintered body 9. The carbon layer is preferably made of conductive carbon. The carbon layer can be formed, for example, by applying a conductive carbon paste to the surface of a metal foil used as a current collector.
[0021] An enclosed space is formed inside the exterior body 24. The electrodes 5 and the electrolyte solution 22 are accommodated in this enclosed space. In the lithium-ion battery 10, the electrolyte solution 22 is sealed inside the exterior body 24. The positive electrode layer 12, the negative electrode layer 16, and the separator 20 are impregnated with the electrolyte solution 22.
[0022] The exterior body 24 may be selected appropriately depending on the type of lithium-ion battery 10. For example, when the lithium-ion battery 10 is in the form of a coin battery as shown in FIG. 1 , the exterior body 24 typically includes a positive electrode can 24a, a negative electrode can 24b, and a gasket 24c, and the positive electrode can 24a and the negative electrode can 24b are crimped together via the gasket 24c to form a sealed space. The positive electrode can 24a and the negative electrode can 24b may be made of a metal such as stainless steel, but are not limited to this. The gasket 24c may be an annular member made of an insulating resin such as polypropylene, polytetrafluoroethylene, or PFA resin, but is not particularly limited to this.
[0023] Although the lithium ion battery 10 shown in FIG. 1 is in the form of a coin battery, the form of the lithium ion battery according to the present disclosure is not limited to a coin battery. For example, other forms, such as a thin secondary battery including a chip-type secondary battery or a pouch-type secondary battery, may also be used. When the lithium ion battery is a chip-type battery that can be built into a card, the exterior body is preferably a resin substrate, and the electrodes and electrolyte are embedded within the resin substrate. For example, when the lithium ion battery is a pouch-type secondary battery, the electrodes may be sandwiched between a pair of resin films. The pair of resin films may be bonded together with an adhesive. Furthermore, the pair of resin films may be heat-sealed together using a heat press. Furthermore, a separator made of a solid electrolyte may be used as the separator, and may not contain an electrolyte.
[0024] (Laminate Section) A laminate section included in a lithium-ion battery according to the present disclosure will now be described. FIG. 2 is a schematic cross-sectional perspective view showing a laminate section 1 as a component of an electrode included in a lithium-ion battery according to the present disclosure. Referring to FIG. 2, the laminate section 1 is a laminate formed by stacking a number of layers. Note that while FIG. 2 shows the laminate section 1 as having a rectangular parallelepiped shape, the shape of the laminate section 1 is not limited to this. It is also preferable that a portion of the periphery is formed in an arc shape to match the desired electrode shape, etc. The laminate section 1 shown in FIG. 2 has a rectangular parallelepiped shape whose outer shape is defined by a width W, a depth D, and a thickness T. Note that the rectangular parallelepiped shape does not only mean a rectangular parallelepiped in the mathematically precise sense, but also includes a three-dimensional structure having a shape similar to a rectangular parallelepiped for design and manufacturing reasons.
[0025] Referring to Figure 2, separators 20 are exposed on the upper and lower surfaces of laminate 1. That is, the uppermost and lowermost layers of laminate 1 are both layers of separator 20. In laminate 1, a positive electrode layer 12 and a negative electrode layer 16 that face each other via separator 20 form one cell. Five cells are formed in laminate 1 in Figure 2. The number of cells in the laminate included in the lithium ion battery according to the present disclosure is not limited as long as the effects of the invention are achieved, but the laminate may include, for example, 3 to 200 cells.
[0026] In the laminate 1, multiple positive electrode layers 12 and multiple negative electrode layers 16 are alternately stacked. The positive electrode layers 12 and negative electrode layers 16 constituting the laminate 1 are each rectangular plate-shaped. The widths of the positive electrode layers 12 and negative electrode layers 16 are both smaller than the width W of the laminate 1. That is, the positive electrode layers 12 and negative electrode layers 16 do not extend across the entire width W of the laminate 1. The positive electrode layers 12 and negative electrode layers 16 are positioned offset from each other in the width direction, and each of the positive electrode layers 12 and negative electrode layers 16 is exposed only on one of the opposing first side surface s1 and second side surface s2 of the laminate 1. Specifically, each of the multiple positive electrode layers 12 is exposed on the first side surface s1 of the laminate 1 but not on the second side surface s2. The positive electrode layer 12 extends from the side surface s1 to the middle of the width direction of the laminate 1, with the inner end surface 12e being its widthwise end. Each of the plurality of negative electrode layers 16 is exposed on the second side surface s2 of the laminated unit 1, but not on the first side surface s1. The negative electrode layer 16 extends in the width direction from the side surface s2 to the middle of the width direction of the laminated unit 1, with the inner end surface 16e being the end in the width direction.
[0027] The negative electrode layer 16 includes a negative electrode current collector layer 19 in contact with the negative electrode layer 16 on one of its main surfaces or inside in the thickness direction. By including the negative electrode current collector layer 19, it is possible to reduce the internal resistance of the laminate portion 1, particularly in the negative electrode layer 16. The negative electrode current collector layer 19 may be provided inside the negative electrode layer 16 in the thickness direction. Alternatively, the negative electrode current collector layer 19 may be formed so as to be exposed on one of the main surfaces of the negative electrode layer 16. The negative electrode current collector layer 19 is made of a material with excellent electrical conductivity.
[0028] A separator 20 is interposed between the positive electrode layer 12 and the negative electrode layer 16. The separator 20 includes a first region 21, a second region 22, and a third region 23. The first region 21 extends across the entire width W of the laminate 1 in the width direction and is interposed between the positive electrode layer 12 and the negative electrode layer 16 in the thickness direction of the laminate 1. The second region 22 is located at the same position as the positive electrode layer 12 in the thickness direction, aligned with the positive electrode layer 12 in the width direction (X-axis direction), and extends between the inner end surface 12e of the positive electrode layer 12 and the side surface s2. The second region 22 functions as an insulating layer that provides insulation between the positive electrode layer 12 and the side surface s2. The third region 23 is located at the same position as the negative electrode layer 16 in the thickness direction, aligned with the negative electrode layer 16 in the width direction (X-axis direction), and extends between the inner end surface 16e of the negative electrode layer 16 and the side surface s1. The third region 23 functions as an insulating layer that provides insulation between the negative electrode layer 16 and the side surface s1. The first region 21, the second region 22, and the third region 23 are continuous without any boundaries. The first region 21, the second region 22, and the third region 23 are regions that are partitioned for the sake of convenience of explanation, and in an actual electrode, it is preferable that the first region 21, the second region 22, and the third region 23 have an integral structure that is continuous throughout.
[0029] (Sintered body) A sintered body included in a lithium ion battery according to the present disclosure will be described. Fig. 3 is a schematic perspective view showing a sintered body 9 included in a lithium ion battery according to the present disclosure. Fig. 3(a) shows the appearance, and Fig. 3(b) is a schematic diagram showing the configuration of layers included in the sintered body 9, including the interior.
[0030] 3(b), the sintered body 9 includes the laminated portion 1 described above and an insulating layer 51 added in contact with the laminated portion 1. Referring to FIGS. 3(a) and 3(b), the positive electrode layer 12 and the separator 20 are exposed on a first side surface s1 of the periphery of the laminated portion 1, but the negative electrode layer 16 is not exposed. The negative electrode layer 16 and the separator 20 are exposed on a second side surface s2 of the periphery of the laminated portion 1, but the positive electrode layer 12 is not exposed. In the sintered body 9, the first side surface s1 and the second side surface s2 of the laminated portion 1 are exposed and form the surface of the sintered body 9.
[0031] 3(b), a laminated structure including a positive electrode layer, a negative electrode layer, and a separator appears on the third side surface s3 and the fourth side surface s4 of the periphery of the laminated portion 1. In the sintered body 9, the third side surface s3 and the fourth side surface s4 of the laminated portion 1 are covered with an insulating layer 51 as an insulating ceramic portion. That is, the third side surface s3 and the fourth side surface s4 of the laminated portion 1 are not exposed to the outside because they are covered with the insulating layer 51 in the sintered body 9. The periphery of the laminated portion 1 refers to the surfaces of the laminated portion 1 located on the periphery, excluding the upper and lower surfaces in the stacking direction.
[0032] The insulating layer 51 is preferably provided so as to cover both the third side surface s3 and the fourth side surface s4 of the laminated portion 1, but may alternatively cover either the third side surface s3 or the fourth side surface s4. Also, it is preferable to cover the entire surfaces of the third side surface s3 and the fourth side surface s4, but it may alternatively cover only a portion of them. The insulating layer 51 extends over at least a portion of the third side surface s3 and the fourth side surface s4 in the stacking direction so as to cover at least some of the layers constituting the stack. Furthermore, the insulating layer 51 is not an essential component, and the sintered body 9 may be composed of only the laminated portion 1.
[0033] In the example shown in Fig. 3, the sintered body 9 has a rectangular parallelepiped (quadrilateral) shape, but the external shape of the sintered body is not limited to this. For example, it may have a cylindrical (round) shape with side surfaces, or a polygonal prism shape. Furthermore, the insulating layer 51 may cover only a portion of the third side surface s3 and the fourth side surface s4, rather than covering the entire third side surface s3 and the fourth side surface s4.
[0034] The sintered body included in the lithium-ion battery according to the present disclosure may be round, in addition to a rectangular shape like the sintered body 9. FIGS. 4( a) and 4(b) show a sintered body 91 having a cylindrical shape with a portion cut away. FIG. 4(a) shows the external appearance, and FIG. 4(b) is a schematic diagram showing the configuration of the layers included in the sintered body 91, including the interior. This shape is referred to as a "round shape." Although the shape of the sintered body 91 differs from that of the sintered body 9, it has the same laminated structure as the sintered body 9. Referring to FIG. 4(b), the sintered body 91 includes a laminated section 11 and an insulating layer 511 arranged to cover the arc-shaped side surface of the laminated section 11. The laminated section 11 has the same configuration as the laminated section 1 except for the different external shape. As shown in FIG. 4, the sintered body 91 has a cylindrical shape with a portion cut away parallel to the tangent, forming two opposing side surfaces s5 and s6. The end surface of the separator 120 and the end surface of the positive electrode layer 112 are exposed on side surface s5. The negative electrode layer 116 is not exposed on the side surface s5. The end surface of the separator 120 and the end surface of the negative electrode layer 116 are exposed on the side surface s6 opposite to the side surface s5. The positive electrode layer 112 is not exposed on the side surface s6.
[0035] Next, the layers included in the electrodes of the lithium ion battery according to the present disclosure and the composition and configuration of the electrolyte in the lithium ion battery will be described.
[0036] (Positive Electrode Layer) The positive electrode layer is made of a sintered body containing lithium cobalt oxide. The positive electrode layer may contain no binder or conductive additive. Specific examples of lithium cobalt oxide include LiCoO 2 (hereinafter, sometimes abbreviated as LCO). Examples of LCO sintered bodies formed into a plate shape include those disclosed in Japanese Patent No. 5587052 and International Publication No. WO 2017 / 146088. The positive electrode layer is preferably an oriented positive electrode layer containing a plurality of primary particles composed of lithium cobalt oxide, the plurality of primary particles being oriented at an average orientation angle of more than 0° and not more than 30° relative to the layer surface of the positive electrode layer. Examples of the structure, composition, and method of specifying such an oriented positive electrode layer include those disclosed in Patent Document 1 (WO 2019 / 221144).
[0037] In addition to LCO, other lithium cobalt oxides that form the primary particles in the positive electrode layer include, for example, Li x NiCoO 2 (lithium nickel cobalt oxide), Li x CoNiMnO 2 (Lithium cobalt-nickel-manganese oxide), Li x CoMnO 2 (lithium cobalt manganese oxide), etc. In addition to the lithium cobalt oxide, other lithium composite oxides may be contained. Examples of the lithium composite oxide include Li x MO 2 (wherein 0.05<x<1.10, and M is at least one transition metal, and M typically includes one or more of Co, Ni, and Mn).
[0038] When the positive electrode layer is made of a plate-shaped sintered body containing LCO, the transition metal element among the elements constituting the positive electrode layer is Co. x NiCoO 2 When the positive electrode layer is made of a sintered body containing lithium nickel-cobalt oxide (LiCoO), the transition metal elements among the elements constituting the positive electrode layer are Ni and Co. x CoNiMnO 2 When the positive electrode layer is made of a sintered body containing lithium cobalt-nickel-manganese oxide (LiFePO), the transition metal elements among the elements constituting the positive electrode layer are Ni, Co, and Mn. This also applies to positive electrodes other than those based on lithium cobalt oxide. For example, when the positive electrode is made of LiFePO 4 When the positive electrode layer is made of lithium iron phosphate, the transition metal element among the elements constituting the positive electrode layer is Fe. The transition metal element constituting the positive electrode layer may be a transition metal element such as V (vanadium).
[0039] The average particle size of the primary particles constituting the positive electrode layer is preferably 5 μm or more. Specifically, the average particle size of the primary particles used to calculate the average orientation angle is preferably 5 μm or more, more preferably 7 μm or more, and even more preferably 12 μm or more.
[0040] The positive electrode layer may contain pores. When the sintered body contains pores, particularly open pores, the electrolyte can penetrate into the sintered body when incorporated into a battery as a positive electrode layer, thereby improving lithium ion conductivity. The porosity of the positive electrode layer is preferably 20 to 60%, more preferably 25 to 55%, and even more preferably 30 to 50%. The porosity of the sintered body can be measured according to a known method.
[0041] The average pore diameter of the positive electrode layer is preferably 0.1 to 10.0 μm, more preferably 0.2 to 5.0 μm, and even more preferably 0.25 to 3.0 μm. Within this range, localized stress concentration in large pores is suppressed, and stress within the sintered body is more easily released uniformly. Furthermore, the lithium ion conductivity can be more effectively improved by the internal penetration of the electrolyte solution through the pores.
[0042] The thickness of the positive electrode layer in the laminated portion is not particularly limited, but is preferably 1 to 200 μm, more preferably 2 to 150 μm, and even more preferably 5 to 100 μm. Within such ranges, electronic resistance is suppressed, and the migration resistance of Li ions contained in the electrolyte is also suppressed, thereby reducing battery resistance.
[0043] (Separator) The separator is made of a ceramic microporous film. 2 (lithium aluminate), LiAlO 2 The separator preferably comprises LiAlO 2 It is a sintered body of LiAlO 2 Conventionally, it has not been envisaged that the material would be used as a separator in a multilayer ceramic electrode.
[0044] LiAlO in the separator 2 The content of may be 50% by volume or more, more preferably 70% by volume or more, and even more preferably 100% by volume. 2 The separator is preferably made of LiAlO (lithium aluminate). 2In addition to the above, other metal oxides can be contained. Specific examples of other metal oxides include MgO, Li 2 ZrO 3 , ZrO 2 , Al 2 O 3 , Li 3 AlO 4 and LiAl 5 O 8 In addition to metal oxides, ceramic materials such as nitrides and carbides, specifically, SiC, Si 3 N 4 , AlN, etc.
[0045] The thickness of the separator in the laminated portion is not particularly limited, but is preferably 1 to 50 μm, and more preferably 2 to 30 μm. The separator thickness here refers to the thickness of the region separating the positive electrode layer and the negative electrode layer in the lamination direction (first region 21 shown in FIG. 2). The second region 22 and third region 23 of the separator 20 can be made to have the same thickness as the positive electrode layer and the negative electrode layer, respectively. The porosity of the separator is not particularly limited, but can be, for example, approximately 30 to 70%, and preferably approximately 40 to 60%.
[0046] (Negative electrode layer) The negative electrode layer is, for example, a plate-shaped sintered body containing a titanium-containing composition. The negative electrode layer may contain no binder or conductive additive. The titanium-containing sintered body may be lithium titanate Li 4 Ti 5 O 12 (hereinafter referred to as LTO) or niobium titanium composite oxide Nb 2 TiO 7 It is preferable that the battery contains Li, and more preferably contains LTO. Although LTO is typically known to have a spinel structure, it can also have other structures during charging and discharging. For example, LTO can have Li 4 Ti 5 O 12 (spinel structure) and Li 7 Ti 5 O 12The reaction proceeds in the coexistence of two phases, i.e., a spinel structure and a rock salt structure. Therefore, LTO is not limited to a spinel structure. LTO may be partially substituted with other elements. Examples of other elements include Nb, Ta, W, Al, and Mg. An LTO sintered body can be produced, for example, according to the method described in JP 2015-185337 A.
[0047] When the negative electrode layer is made of a sintered body containing LTO, the transition metal element among the elements constituting the negative electrode layer is Ti. 2 TiO 7 When the negative electrode layer is made of a sintered body containing Nb and Ti, the transition metal elements among the elements constituting the negative electrode layer are Nb and Ti.
[0048] The negative electrode layer has a structure in which a large number of primary particles are bonded together. These primary particles are made of LTO or Nb 2 TiO 7 The negative electrode layer is preferably configured as an integral sintered body together with the positive electrode layer and the separator 20 .
[0049] The thickness of the negative electrode layer is not particularly limited, but is, for example, preferably 1 to 200 μm, more preferably 2 to 150 μm, and even more preferably 5 to 100 μm. The primary particle size, which is the average particle size of the multiple primary particles constituting the negative electrode layer, is preferably 1.2 μm or less, more preferably 0.02 to 1.2 μm, and even more preferably 0.05 to 0.7 μm.
[0050] The negative electrode layer preferably contains pores. By containing pores, particularly open pores, when the negative electrode layer is incorporated into a battery, the electrolyte can penetrate into the inside, resulting in improved lithium ion conductivity. The porosity of the negative electrode layer is preferably 20 to 60%, more preferably 30 to 55%, and even more preferably 35 to 50%. The average pore diameter of the negative electrode layer is preferably 0.08 to 5.0 μm, more preferably 0.1 to 3.0 μm, and even more preferably 0.12 to 1.5 μm.
[0051] (Negative Electrode Current Collector Layer) The negative electrode current collector layer can be made of a material with excellent conductivity. In the lithium-ion battery according to the present disclosure, the negative electrode current collector layer contains Ag (silver). In addition to Ag, the negative electrode current collector layer may further contain one or more elements selected from the group consisting of Au (gold), Pt (platinum), Pd (palladium), Al (aluminum), Cu (copper), and Ni (nickel). The Ag content in the negative electrode current collector layer may be 30% or more, more preferably 50% or more, and even more preferably 100%. In other words, the negative electrode current collector layer 19 is preferably a layer made of Ag.
[0052] The thickness of the negative electrode current collector layer is not particularly limited, but is preferably 0.1 to 60 μm, more preferably 0.5 to 30 μm. It is believed that when the relationship between the thickness of the negative electrode current collector layer and the thickness of the separator is within a certain range, the diffusion of Ag contained in the negative electrode current collector layer can be effectively suppressed. Specifically, the ratio of the thickness of the negative electrode current collector layer (A) to the thickness of the separator (B) preferably satisfies 0.1≦B / A≦50, and more preferably 0.15≦B / A≦30.
[0053] (Insulating ceramic portion) The insulating layer included in the sintered body covers the periphery of the laminated portion, particularly the side surfaces other than the portions where the internal electrode layers are drawn out. The insulating layer is made of insulating ceramic. Specifically, the same ceramic as that used as the separator can be used. The insulating ceramic portion can be made of LiAlO 2 LiAlO 2 It is preferable that the insulating layer is made of a material selected from the group consisting of propylene, propylene, propylene, propylene- ...
[0054] (Electrolyte) The lithium ion battery contains an electrolyte. The electrolyte is not particularly limited, and any electrolyte known as an electrolyte for lithium ion batteries can be used. For example, the solvent can be one or a combination of two or more selected from ethylene carbonate (EC), methyl ethyl carbonate (MEC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), propylene carbonate (PC), and γ-butyrolactone (GBL). The electrolyte dissolved in the solvent can be, for example, lithium hexafluorophosphate (LiPF 6 ), lithium fluoride (LiBF 4 The electrolyte solution 22 may further contain at least one additive selected from vinylene carbonate (VC), fluoroethylene carbonate (FEC), vinylethylene carbonate (VEC), and lithium difluoro(oxalato)borate (LiDFOB).
[0055] The concentration of the electrolyte in the electrolytic solution is preferably 0.5 to 4.0 mol / L, more preferably 0.6 to 3.0 mol / L, even more preferably 0.7 to 2.5 mol / L, and particularly preferably 0.8 to 2.0 mol / L.
[0056] In addition to an electrolytic solution, a solid electrolyte or a polymer electrolyte can also be used as the electrolyte. In this case, as with an electrolytic solution, it is preferable that the electrolyte is impregnated at least into the pores of the separator. The impregnation method is not particularly limited, but examples include a method in which the electrolyte is melted and infiltrated into the pores of the separator, and a method in which a powder compact of the electrolyte is pressed against the separator.
[0057] (Manufacturing Method) An outline of a manufacturing method of a sintered body included in a lithium ion battery according to the present disclosure will be described. Fig. 5 shows a schematic diagram of the manufacturing process of a sintered body, in which each sheet for constituting a laminate is prepared, stacked, and pressure-bonded.
[0058] Referring to FIG. 5(1), the positive electrode green sheet 112, the negative electrode green sheet 116, and the separator green sheet 120, which are the materials constituting the laminate, are each prepared separately. Typically, the green sheets can be prepared by first preparing a slurry containing the raw materials constituting each layer, and then forming the prepared slurry into a sheet on a resin film. The negative electrode green sheet 116 may have a current collector layer 119 formed on one of its main surfaces. Referring to FIG. 5(2), each sheet is cut to a predetermined width and stacked in order to form a predetermined layer structure. Note that while the example in FIG. 5 simply illustrates the layer structure, a unit U including the negative electrode green sheet 116, the separator green sheet 120, the positive electrode green sheet 112, and the separator green sheet 120 may be repeatedly stacked to form a multi-layer laminate.
[0059] Referring to FIG. 5(1), when stacking, each green sheet may be used alone in the thickness direction, or two or more sheets of the same type may be continuously stacked in the thickness direction. For example, to form the negative electrode layer 16, two negative electrode green sheets 116 having a current collector layer 119 on one side may be stacked. When two negative electrode green sheets 116 having a current collector layer 119 are stacked, it is preferable to stack them so that the current collector layers 119 are in contact with each other. When two or more sheets of the same type are stacked in the thickness direction, the stacked sheets are integrated during the sintering stage, resulting in a single layer in the sintered body. Referring to FIG. 5(2), when stacking, the positive electrode green sheet 112 and the negative electrode green sheet 116 are arranged so that they are offset from each other in the width direction (X-axis direction). By arranging them in this manner, it is possible to obtain a configuration in which, of the pair of side surfaces of the laminate 1 (FIG. 2), the positive electrode layer 12 is exposed on one side surface but the negative electrode layer 16 is not exposed, and the negative electrode layer 16 is exposed on the other side surface but the positive electrode layer 12 is not exposed.
[0060] Referring to Fig. 5 (3), the green sheet laminate 101 is pressed to pressure-bond the layers together. Specifically, the green sheets included in the green sheet laminate 101 can be pressure-bonded together by pressing. It is preferable to press the green sheet laminate 101 in the thickness direction (Z-axis direction). The pressing method can be, for example, cold isostatic pressing (CIP), hot isostatic pressing (WIP), hydrostatic pressing, or the like, and is not particularly limited. Pressing may be performed while heating.
[0061] Next, the green sheet laminate 101 is cut. FIG. 6 shows part of the process for producing a rectangular sintered body in which each layer is formed as a quadrilateral and the entire body is a rectangular parallelepiped. In FIG. 6(1), cutting locations c1 to c4 are indicated by thick lines. Referring to FIG. 6(1), first, both side surfaces of the green sheet laminate 101 are cut at cutting locations c1 and c2 to obtain a predetermined width. Cutting location c1 is a location where the positive electrode green sheet 112 is cut but the negative electrode green sheet 116 is not cut. Cutting location c2 is a location where the negative electrode green sheet 116 is cut but the positive electrode green sheet 112 is not cut. Next, the front and back surfaces of the green sheet laminate 101 are cut at cutting locations c3 and c4. Cutting locations c3 and c4 are locations where only the separator green sheet 120 is cut but the positive electrode green sheet 112 and the negative electrode green sheet 116 are not cut. Next, degreasing and firing are carried out to obtain an integrated sintered body 9 (FIG. 6(2)) having an insulating ceramic portion on the periphery of the laminate. The degreasing and firing can be carried out under known conditions and by known methods.
[0062] FIG. 7 shows a green sheet laminate 911 for obtaining a round sintered body. The green sheet laminate 911 is obtained by cutting out a positive electrode green sheet 112, a negative electrode green sheet 116, and a separator green sheet 120 into a circular shape using a punch or the like. FIG. 7(1) is a schematic diagram showing the internal layer structure of the green sheet laminate 911. The positive electrode green sheet 112, the negative electrode green sheet 116, and the separator green sheet 120 that constitute the respective layers of the green sheet laminate 911 can be the same as the various green sheets that constitute the green sheet laminate 101, except for their shapes. The layering order can also be the same as that of the green sheet laminate 101.
[0063] 7(1), each of the positive electrode green sheets 112 and the negative electrode green sheets 116 included in the green sheet laminate 911 has a shape in which a portion of a circle has been cut away parallel to the tangent. The positive electrode green sheets 112 and the negative electrode green sheets 116 are alternately stacked with circular separator green sheets 120 interposed therebetween. The positive electrode green sheets 112 and the negative electrode green sheets 116 are arranged such that the cut portions are located on opposite sides of each other. Furthermore, the separator green sheets 120 cover the entire periphery of the stacked portion.
[0064] After the green sheet laminate 911 is stacked and pressed, the green sheet laminate 911 is cut. In FIG. 7(1), cut locations c8 and c9 are indicated by bold lines. Referring to FIG. 7(1), cut location c8 is a position where the positive electrode green sheet 112 is cut and does not overlap with the negative electrode green sheet 116. Furthermore, cut location c8 is parallel to the cut portion of the negative electrode green sheet 116. By cutting the green sheet laminate 911 at this position, a side surface s5 (FIG. 7(2)) is obtained in which the positive electrode green sheet 112 and the separator green sheet 120 are exposed in the cross section and the negative electrode green sheet 116 is not exposed. Cut location c9 is a position where the negative electrode green sheet 116 is cut and does not overlap with the positive electrode green sheet 112. Furthermore, cut location c9 is parallel to the cut portion of the positive electrode green sheet 112. By cutting green sheet laminate 911 at this position, a side surface s6 ( FIG. 7(2) ) is obtained in which negative electrode green sheet 116 and separator green sheet 120 are exposed in the cross section, but positive electrode green sheet 112 is not exposed. Next, degreasing and firing are performed, and an integrated sintered body 91 is obtained in which an insulating ceramic portion is formed around the periphery of the laminate portion.
[0065] Once the sintered body is obtained, current collectors are then attached to both sides of the sintered body. For example, referring to FIG. 1 , a positive electrode current collector 14 is attached to the first side surface s1 of the sintered body 9, and a negative electrode current collector 18 is attached to the second side surface s2. A conductive material, such as aluminum foil, can be used for the positive electrode current collector 14 and the negative electrode current collector 18. The positive electrode current collector 14 is attached to cover the entire first side surface s1 and can extend onto the lower surface of the sintered body 9. The negative electrode current collector 18 is attached to cover the entire second side surface s2 and can extend onto the upper surface of the sintered body 9. The sintered body 9 and the positive electrode current collector 14, and the sintered body 9 and the negative electrode current collector 18 can be bonded together using a conductive adhesive. For example, a conductive carbon paste can be used as the conductive adhesive. The thickness of the conductive adhesive layer is not particularly limited as long as it exhibits its effect as an adhesive layer and does not impede the effects of the invention, but it can be, for example, about 1 to 500 μm.
[0066] The electrode obtained by the above-described manufacturing method can be housed inside an exterior body according to known methods and conditions, and an electrolyte solution can be sealed in to obtain a lithium ion battery.
[0067] [Examples and Comparative Examples] The lithium ion battery of the present disclosure will be described in more detail below with reference to Examples and Comparative Examples. Samples 1 to 7 are examples of lithium ion batteries according to the present disclosure. Samples 8 and 9 are comparative examples that are outside the scope of the lithium ion battery according to the present disclosure.
[0068] [Sample 1] A lithium ion battery was fabricated according to the methods described in 1 to 8 below.
[0069] 1. Preparation of Laminate Green sheets for each layer constituting the sintered body were prepared under the conditions and methods of (1) to (3). In (1) to (3), the viscosity of the slurry was measured using a Brookfield LVT viscometer. The doctor blade method was used to cast the slurry onto a PET film.
[0070] (1) Preparation of LCO green sheet (positive electrode green sheet) Co was weighed so that the Li / Co molar ratio was 1.01. 3 O 4 Powder (manufactured by Seido Chemical Industry Co., Ltd.) and Li 2 CO 3 The powder (manufactured by Honjo Chemical Co., Ltd.) was mixed and then held at 780° C. for 5 hours. The obtained powder was milled in a pot mill to a volumetric standard D 50The powder was pulverized to a particle size of 0.4 μm to obtain a powder composed of LCO plate-like particles. 100 parts by weight of the obtained LCO powder, 100 parts by weight of a dispersion medium (toluene:isopropanol=1:1), 10 parts by weight of a binder (polyvinyl butyral: product number BM-2, manufactured by Sekisui Chemical Co., Ltd.), 2 parts by weight of a plasticizer (DOP: Di(2-ethylhexyl) phthalate, manufactured by Kurogane Kasei Co., Ltd.), and 4.5 parts by weight of a dispersant (product name: Rheodor SP-O30, manufactured by Kao Corporation). The resulting mixture was stirred under reduced pressure to degas and the viscosity was adjusted to 4000 cP to prepare an LCO slurry. The prepared slurry was formed into a sheet on a PET film to form an LCO green sheet. The thickness of the positive electrode layer after firing was adjusted to 24 μm.
[0071] (2) Preparation of LTO green sheet (negative electrode green sheet) LTO powder (volume basis D 50 100 parts by weight of a 0.6 μm particle size (manufactured by Ishihara Sangyo Kaisha, Ltd.), 100 parts by weight of a dispersion medium (toluene:isopropanol=1:1), 10 parts by weight of a binder (polyvinyl butyral: product number BM-2, manufactured by Sekisui Chemical Co., Ltd.), 2 parts by weight of a plasticizer (DOP: Di(2-ethylhexyl) phthalate, manufactured by Kurogane Kasei Co., Ltd.), and 2 parts by weight of a dispersant (product name: Rheodol SP-O30, manufactured by Kao Corporation) were mixed. The resulting negative electrode raw material mixture was stirred under reduced pressure to degas and the viscosity was adjusted to 4000 cP to prepare an LTO slurry. The prepared slurry was formed into a sheet on a PET film to form an LTO green sheet. The thickness of the negative electrode layer after firing was adjusted to 10 μm.
[0072] (2') Formation of negative electrode current collector layer: Ag paste (product name: NP423C1, manufactured by Tanaka Kikinzoku Kogyo Co., Ltd.) was printed on one side of the LTO green sheet prepared in (2) using a printer. The thickness of the printed layer was adjusted to 5 μm after firing.
[0073] (3) Preparation of separator green sheet and insulating layer green sheet Li 2 CO 3 Powder (manufactured by Honjo Chemical Co., Ltd.) and Al2 O 3 (manufactured by Sumitomo Chemical Co., Ltd., product name: AKP-20) was mixed so that the molar ratio of Li / Al was 1.00, and then heat-treated at 900°C for 5 hours to obtain LiAlO 2 A powder of LiAlO was obtained. 2 Powder (volume basis D 50 100 parts by weight of 1.5 μm particle diameter, 100 parts by weight of a dispersion medium (toluene:isopropanol = 1:1), 20 parts by weight of a binder (polyvinyl butyral: product number BM-2, manufactured by Sekisui Chemical Co., Ltd.), 4 parts by weight of a plasticizer (DOP: Di(2-ethylhexyl) phthalate, manufactured by Kurogane Kasei Co., Ltd.), and 2 parts by weight of a dispersant (product name: Rheodor SP-O30, manufactured by Kao Corporation) were mixed. The resulting raw material mixture was stirred under reduced pressure to degas and the viscosity was adjusted to 4000 cP to prepare a slurry. The prepared slurry was formed into a sheet on a PET film to form a separator green sheet. The thickness of the separator located between the positive electrode layer and the negative electrode layer was adjusted to 25 μm after firing. The thickness of the separator (insulating layer) located next to the positive electrode layer was adjusted to the same thickness as the positive electrode layer after firing. The thickness of the separator (insulating layer) located next to the negative electrode layer was set to be the same as the thickness of the negative electrode layer and the current collector layer after firing.
[0074] 2. Cutting the Sheets The green sheets obtained in step 1 were cut to be stacked. Specifically, the positive electrode green sheet and the negative electrode green sheet were each punched out with a round puncher having a diameter of 15.5 mm to obtain circular green sheets. Furthermore, each circular green sheet was cut linearly at a position 2 mm from one point on the edge toward the center, parallel to the tangent line at that point.
[0075] 3. Stacking, Compression, and Cutting of the Laminate Next, various green sheets were stacked in the stacking order shown in [Figure 5] (1) so that the number of cells formed in the laminate would be 15. As shown in [Figure 7], the cut end faces of the positive electrode green sheet and the negative electrode green sheet were positioned opposite each other across the center of the circle. Next, the green sheet laminate was pressed to compress the green sheets together. The compressed green sheet laminate was punched out using a hand punch with a diameter of 16 mm. Furthermore, as shown in [Figure 7], two cuts were made along two parallel lines. The cut positions were such that the positive electrode and separator were exposed on one end face but the negative electrode layer was not exposed, and the negative electrode layer was exposed on the other end face but the negative electrode layer was not exposed.
[0076] 4. Degreasing and Firing Next, the cut laminate was heated from room temperature to 600°C and degreased for 5 hours, then heated to 800°C and held for 10 minutes to be fired, and then cooled. Aluminum foil was placed as a positive electrode current collector on the surface where the positive electrode and separator were exposed, with conductive carbon paste interposed therebetween. Furthermore, aluminum foil was placed as a negative electrode current collector on the surface where the negative electrode and separator were exposed, with conductive carbon paste interposed therebetween.
[0077] 5. Preparation of Conductive Carbon Paste A binder (CMC: MAC350HC, manufactured by Nippon Paper Industries Co., Ltd.) was weighed out to 1.2 wt% in pure water and dissolved using a stirrer to obtain a 1.2 wt% CMC solution. A carbon dispersion (product number: BPW-229, manufactured by Nippon Graphite Co., Ltd.) and a dispersant solution (product number LB-300, manufactured by Showa Denko K.K.) were prepared. Next, the carbon dispersion, dispersant solution, and 1.2 wt% CMC solution were weighed out to a ratio of 0.22:0.29:1, and these were mixed using a planetary mixer to prepare a conductive carbon paste.
[0078] 6. Bonding the exposed positive electrode surface of the laminated integrated sintered body to aluminum foil with conductive carbon paste The conductive carbon paste obtained in 5. was screen-printed onto aluminum foil as a positive electrode current collector. The laminated integrated sintered body obtained in 4. was placed so that the exposed positive electrode surface was adhered within the undried print pattern (the area where the conductive carbon paste was applied), and after lightly pressing with a finger, it was vacuum-dried at 50°C for 60 minutes. In this way, the exposed positive electrode surface of the laminated integrated sintered body and the positive electrode current collector were bonded via a conductive carbon adhesive layer. The thickness of the conductive carbon adhesive layer was 30 μm.
[0079] 7. Bonding the exposed negative electrode surface of the laminated integrated sintered body to aluminum foil with conductive carbon paste In the same manner as in 6, aluminum foil was bonded as a negative electrode current collector to the exposed negative electrode surface of the laminated integrated sintered body via a conductive carbon adhesive layer.
[0080] 8. Fabrication of Lithium-ion Battery A positive electrode current collector, a sintered laminate, and a negative electrode current collector were stacked in this order between the positive electrode can and the negative electrode can, which would form the battery case. After filling with electrolyte, the positive electrode can and the negative electrode can were sealed by crimping them together with a gasket. In this way, a coin-cell type lithium-ion battery with a diameter of 20 mm and a thickness of 1.6 mm was fabricated. [Figure 8] shows a schematic perspective view of the exterior of the lithium-ion battery. The electrolyte was an organic solvent made by mixing propylene carbonate (PC) and gamma-butyrolactone (GBL) in a volume ratio of 1:3, and LiPF 6 was dissolved to a concentration of 1.5 mol / L.
[0081] [Sample 2] LiAlO as a separator 2 A lithium ion battery was fabricated in the same manner as in Sample 1, except that a material containing LiAlO and MgO was used. 2 Preparation of separator green sheets and insulating layer green sheets containing Li and MgO 2 CO 3 Powder (manufactured by Honjo Chemical Co., Ltd.) and Al 2 O 3(manufactured by Sumitomo Chemical Co., Ltd., product name: AKP-20) was mixed so that the molar ratio of Li / Al was 1.00, and then heat-treated at 900°C for 5 hours to obtain LiAlO 2 Magnesium carbonate powder (manufactured by Konoshima Chemical Co., Ltd.) was heat-treated at 900°C for 5 hours to obtain MgO powder. 2 The powder and MgO powder were mixed in a volume ratio of 50 vol %:50 vol %. 50 100 parts by weight of a powder (particle size 0.4 μm), 100 parts by weight of a dispersion medium (toluene:isopropanol=1:1), 20 parts by weight of a binder (polyvinyl butyral: product number BM-2, manufactured by Sekisui Chemical Co., Ltd.), 4 parts by weight of a plasticizer (DOP: Di(2-ethylhexyl) phthalate, manufactured by Kurogane Kasei Co., Ltd.), and 2 parts by weight of a dispersant (product name: Rheodol SP-O30, manufactured by Kao Corporation) were mixed together. The resulting raw material mixture was stirred under reduced pressure to degas and the viscosity was adjusted to 4000 cP to prepare a slurry. The prepared slurry was formed into a sheet on a PET film to form a separator green sheet.
[0082] [Sample 3] LiAlO as a separator 2 and Li 2 ZrO 3 A lithium ion battery was fabricated in the same manner as in Sample 1, except that a material containing LiAlO was used. 2 and Li 2 ZrO 3 Preparation of separator green sheet and insulating layer green sheet containing Li 2 CO 3 Powder (manufactured by Honjo Chemical Co., Ltd.) and Al 2 O 3 (manufactured by Sumitomo Chemical Co., Ltd., product name: AKP-20) was mixed so that the molar ratio of Li / Al was 1.00, and then heat-treated at 900°C for 5 hours to obtain LiAlO 2 A powder was obtained. 2 CO 3 Powder (manufactured by Honjo Chemical Co., Ltd.) and ZrO 2 (manufactured by Tosoh Corporation, product name: TZ-0) was mixed so that the molar ratio of Li / Zr was 2.00, and then heat-treated at 900°C for 5 hours to obtain Li.2 ZrO 3 The resulting LiAlO powder 2 Powder and Li 2 The resulting mixed powder (volume basis D 50 100 parts by weight of a powder (particle size 0.4 μm), 100 parts by weight of a dispersion medium (toluene:isopropanol=1:1), 20 parts by weight of a binder (polyvinyl butyral: product number BM-2, manufactured by Sekisui Chemical Co., Ltd.), 4 parts by weight of a plasticizer (DOP: Di(2-ethylhexyl) phthalate, manufactured by Kurogane Kasei Co., Ltd.), and 2 parts by weight of a dispersant (product name: Rheodol SP-O30, manufactured by Kao Corporation) were mixed together. The resulting raw material mixture was stirred under reduced pressure to degas and the viscosity was adjusted to 4000 cP to prepare a slurry. The prepared slurry was formed into a sheet on a PET film to form a separator green sheet.
[0083] [Sample 4] LiAlO as a separator 2 and ZrO 2 A lithium ion battery was fabricated in the same manner as in Sample 1, except that a material containing LiAlO was used. 2 and ZrO 2 Preparation of separator green sheet and insulating layer green sheet containing Li 2 CO 3 Powder (manufactured by Honjo Chemical Co., Ltd.) and Al 2 O 3 (manufactured by Sumitomo Chemical Co., Ltd., product name: AKP-20) was mixed so that the molar ratio of Li / Al was 1.00, and then heat-treated at 900°C for 5 hours to obtain LiAlO 2 The resulting LiAlO powder 2 Powder and ZrO 2 (manufactured by Tosoh Corporation, product name TZ-0) powder was mixed in a volume ratio of 90 VOL%:10 VOL%. 50100 parts by weight of a powder (particle size 0.4 μm), 100 parts by weight of a dispersion medium (toluene:isopropanol = 1:1), 20 parts by weight of a binder (polyvinyl butyral: product number BM-2, manufactured by Sekisui Chemical Co., Ltd.), 4 parts by weight of a plasticizer (DOP: Di(2-ethylhexyl) phthalate, manufactured by Kurogane Kasei Co., Ltd.), and 2 parts by weight of a dispersant (product name: Rheodol SP-O30, manufactured by Kao Corporation) were mixed. The resulting raw material mixture was stirred under reduced pressure to degas and the viscosity was adjusted to 4000 cP to prepare a slurry. The prepared slurry was formed into a sheet on a PET film to form a separator green sheet.
[0084] [Sample 5] LiAlO as a separator 2 and Al 2 O 3 A lithium ion battery was fabricated in the same manner as in Sample 1, except that a material containing LiAlO was used. 2 and Al 2 O 3 Preparation of separator green sheet and insulating layer green sheet containing Li 2 CO 3 Powder (manufactured by Honjo Chemical Co., Ltd.) and Al 2 O 3 (manufactured by Sumitomo Chemical Co., Ltd., product name: AKP-20) was mixed so that the molar ratio of Li / Al was 1.00, and then heat-treated at 900°C for 5 hours to obtain LiAlO 2 The resulting LiAlO powder 2 Powder and Al 2 O 3 The resulting mixed powder (volume basis D 50100 parts by weight of a powder (particle size 0.4 μm), 100 parts by weight of a dispersion medium (toluene:isopropanol = 1:1), 20 parts by weight of a binder (polyvinyl butyral: product number BM-2, manufactured by Sekisui Chemical Co., Ltd.), 4 parts by weight of a plasticizer (DOP: Di(2-ethylhexyl) phthalate, manufactured by Kurogane Kasei Co., Ltd.), and 2 parts by weight of a dispersant (product name: Rheodol SP-O30, manufactured by Kao Corporation) were mixed. The resulting raw material mixture was stirred under reduced pressure to degas and the viscosity was adjusted to 4000 cP to prepare a slurry. The prepared slurry was formed into a sheet on a PET film to form a separator green sheet.
[0085] [Sample 6] LiAlO as a separator 2 and Li 3 AlO 4 A lithium ion battery was fabricated in the same manner as in Sample 1, except that a material containing LiAlO was used. 2 and Li 3 AlO 4 Preparation of separator green sheet and insulating layer green sheet containing Li 2 CO 3 Powder (manufactured by Honjo Chemical Co., Ltd.) and Al 2 O 3 (manufactured by Sumitomo Chemical Co., Ltd., product name: AKP-20) was mixed so that the molar ratio of Li / Al was 1.00, and then heat-treated at 900°C for 5 hours to obtain LiAlO 2 A powder was obtained. 2 CO 3 Powder (manufactured by Honjo Chemical Co., Ltd.) and Al 2 O 3 powder (manufactured by Sumitomo Chemical Co., Ltd., product name: AKP-20) was mixed so that the molar ratio of Li / Al was 3.00, and then heat-treated at 900°C for 5 hours to obtain Li. 3 AlO 4 The resulting LiAlO powder 2 Powder and Li 3 AlO 4 The powder was mixed at a volume ratio of 80 vol %:20 vol %. 50100 parts by weight of a powder (particle size 0.4 μm), 100 parts by weight of a dispersion medium (toluene:isopropanol=1:1), 20 parts by weight of a binder (polyvinyl butyral: product number BM-2, manufactured by Sekisui Chemical Co., Ltd.), 4 parts by weight of a plasticizer (DOP: Di(2-ethylhexyl) phthalate, manufactured by Kurogane Kasei Co., Ltd.), and 2 parts by weight of a dispersant (product name: Rheodol SP-O30, manufactured by Kao Corporation) were mixed together. The resulting raw material mixture was stirred under reduced pressure to degas and the viscosity was adjusted to 4000 cP to prepare a slurry. The prepared slurry was formed into a sheet on a PET film to form a separator green sheet.
[0086] [Sample 7] LiAlO as a separator 2 and LiAl 5 O 8 A lithium ion battery was fabricated in the same manner as in Sample 1, except that a material containing LiAlO was used. 2 and LiAl 5 O 8 Preparation of separator green sheet and insulating layer green sheet containing Li 2 CO 3 Powder (manufactured by Honjo Chemical Co., Ltd.) and Al 2 O 3 (manufactured by Sumitomo Chemical Co., Ltd., product name: AKP-20) was mixed so that the molar ratio of Li / Al was 1.00, and then heat-treated at 900°C for 5 hours to obtain LiAlO 2 A powder was obtained. 2 CO 3 Powder (manufactured by Honjo Chemical Co., Ltd.) and Al 2 O 3 (manufactured by Sumitomo Chemical Co., Ltd., product name: AKP-20) was mixed so that the molar ratio of Li / Al was 0.20, and then heat-treated at 900°C for 5 hours to obtain LiAl 5 O 8 The resulting LiAlO powder 2 Powder and LiAl 5 O 8 The powder was mixed at a volume ratio of 80 vol %:20 vol %. 50100 parts by weight of a powder (particle size 0.4 μm), 100 parts by weight of a dispersion medium (toluene:isopropanol=1:1), 20 parts by weight of a binder (polyvinyl butyral: product number BM-2, manufactured by Sekisui Chemical Co., Ltd.), 4 parts by weight of a plasticizer (DOP: Di(2-ethylhexyl) phthalate, manufactured by Kurogane Kasei Co., Ltd.), and 2 parts by weight of a dispersant (product name: Rheodol SP-O30, manufactured by Kao Corporation) were mixed together. The resulting raw material mixture was stirred under reduced pressure to degas and the viscosity was adjusted to 4000 cP to prepare a slurry. The prepared slurry was formed into a sheet on a PET film to form a separator green sheet.
[0087] [Sample 8] A lithium ion battery was fabricated in the same manner as Sample 1, except that a separator containing MgO and glass frit was used. Preparation of separator green sheet and insulating layer green sheet containing MgO and glass frit: Magnesium carbonate powder (manufactured by Konoshima Chemical Co., Ltd.) was heat-treated at 900°C for 5 hours to obtain MgO powder. The obtained MgO powder and glass frit (manufactured by Nippon Frit Co., Ltd., CK0199) were mixed at a weight ratio of 7:3. The obtained mixed powder (volume basis D 50 100 parts by weight of a powder (particle size 0.4 μm), 100 parts by weight of a dispersion medium (toluene:isopropanol=1:1), 30 parts by weight of a binder (polyvinyl butyral: product number BM-2, manufactured by Sekisui Chemical Co., Ltd.), 6 parts by weight of a plasticizer (DOP: Di(2-ethylhexyl) phthalate, manufactured by Kurogane Kasei Co., Ltd.), and 2 parts by weight of a dispersant (product name: Rheodol SP-O30, manufactured by Kao Corporation) were mixed together. The resulting raw material mixture was stirred under reduced pressure to degas and the viscosity was adjusted to 4000 cP to prepare a slurry. The prepared slurry was formed into a sheet on a PET film to form a separator green sheet.
[0088] [Sample 9] LiAlO as a separator 2 A lithium ion battery was fabricated in the same manner as in Sample 1, except that a material containing LiAlO and MgO was used. 2Preparation of separator green sheets and insulating layer green sheets containing Li and MgO 2 CO 3 Powder (manufactured by Honjo Chemical Co., Ltd.) and Al 2 O 3 (manufactured by Sumitomo Chemical Co., Ltd., product name: AKP-20) was mixed so that the molar ratio of Li / Al was 1.00, and then heat-treated at 900°C for 5 hours to obtain LiAlO 2 Magnesium carbonate powder (manufactured by Konoshima Chemical Co., Ltd.) was heat-treated at 900°C for 5 hours to obtain MgO powder. 2 The powder and MgO powder were mixed in a volume ratio of 30 vol %:70 vol %. 50 100 parts by weight of a powder (particle size 0.4 μm), 100 parts by weight of a dispersion medium (toluene:isopropanol=1:1), 20 parts by weight of a binder (polyvinyl butyral: product number BM-2, manufactured by Sekisui Chemical Co., Ltd.), 4 parts by weight of a plasticizer (DOP: Di(2-ethylhexyl) phthalate, manufactured by Kurogane Kasei Co., Ltd.), and 2 parts by weight of a dispersant (product name: Rheodol SP-O30, manufactured by Kao Corporation) were mixed together. The resulting raw material mixture was stirred under reduced pressure to degas and the viscosity was adjusted to 4000 cP to prepare a slurry. The prepared slurry was formed into a sheet on a PET film to form a separator green sheet.
[0089] [Evaluation] The obtained lithium ion batteries of Samples 1 to 9 were evaluated by the method described in Evaluation 1.
[0090] Evaluation 1. Evaluation of high-temperature charge / discharge properties One hundred lithium-ion batteries were subjected to constant current / low voltage (CCCV) charging (0.1 C / 0.01 C) in an environment of 85° C. If 95% or more (95 or more batteries) of the batteries completed CV charging at 0.01 V, the battery was rated as passed, and if less than 95% (less than 95 batteries) the battery was rated as failed.
[0091] The configurations and evaluation results of the lithium ion batteries of Samples 1 to 9 are summarized in Table 1. In Table 1, "LAO" means LiAlO 2 This means:
[0092]
[0093] As shown in Table 1, the lithium ion batteries of Samples 1 to 7 were all evaluated as "pass" in the high-temperature charge-discharge evaluation. The lithium ion batteries of Samples 1 to 7 used Ag as the negative electrode current collector layer and LiAlO as the separator. 2 It was confirmed that a lithium ion battery using Ag as the negative electrode current collector layer and a sintered body containing lithium aluminate as the separator can reliably charge and discharge even when placed in a high-temperature environment. In contrast, the lithium ion battery of Sample 8 using Ag as the negative electrode current collector layer and a conventional ceramic separator containing MgO and glass as the separator showed insufficient results in the high-temperature charge and discharge evaluation. In addition, the LiAlO 2 The lithium ion battery of Sample 9, in which the ratio of 1 to 30% by volume was 30%, showed insufficient results in the high-temperature charge-discharge evaluation. It is believed that a micro-short circuit or a short circuit occurred inside the electrode at high temperatures.
[0094] It should be understood that the embodiments disclosed herein are illustrative in all respects and are not limiting in any respect. The scope of the present disclosure is defined not by the above description but by the claims, and it is intended to include all modifications within the meaning and scope of the claims.
[0095] REFERENCE SIGNS LIST 1 Laminate, 5 Electrode, 10 Lithium ion battery, 12 Positive electrode layer, 16 Negative electrode layer, 14 Positive electrode current collector, 18 Negative electrode current collector, 19 Negative electrode current collector layer, 20 Separator, 22 Electrolyte, 24 Outer casing, 24a Positive electrode can, 24b Negative electrode can, 24c Gasket, 51, 52 Insulating layer, 9, 91 Sintered body, 101 Green sheet laminate, 112 Positive electrode green sheet, 116 Negative electrode green sheet, 120 Separator green sheet.
Claims
1. An electrode including a plurality of positive electrode layers, a plurality of negative electrode layers, and a separator disposed between the positive electrode layers and the negative electrode layers, the electrode including an integrated sintered body in which the plurality of positive electrode layers, the plurality of negative electrode layers, and the separator are sintered together; an electrolyte impregnated in the electrode; and an exterior body in which the electrode and the electrolyte are housed. In the electrode, a negative electrode current collector layer is provided in contact with the negative electrode layer, the negative electrode current collector layer contains Ag, and the separator is LiAlO 2 and LiAlO in the separator. 2 The content ratio of is 50 volume % or more.
2. The separator is LiAlO 2 and LiAlO 2 and a metal oxide other than the metal oxide of claim 1.
3. The lithium ion battery according to claim 1 or 2, wherein the positive electrode layer is made of a sintered lithium composite oxide, and the negative electrode layer is made of a sintered titanium-containing body.
4. The lithium ion battery according to claim 1 or 2, wherein the negative electrode current collector layer has a thickness of 0.1 μm or more and 60 μm or less, and the separator has a thickness of 1 μm or more and 50 μm or less.
Citation Information
Patent Citations
Positive electrode assembly of lithium ion battery, preparation method thereof and all-solid-state lithium battery
CN110858661A
Lithium-ion secondary battery and method for manufacturing same
WO2021214946A1
Lithium ion secondary battery
WO2022044409A1