Copolymer, positive resist composition, and resist pattern formation method

The use of a copolymer with a LUMO of -0.70 eV or more in the monomer unit and an alcohol-based development process addresses the limitations of conventional resists by enhancing exposure margins and pattern quality in semiconductor manufacturing.

WO2024203960A1PCT designated stage expired Publication Date: 2024-10-03ZEON CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011498
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional main chain cleavage type positive resists in semiconductor manufacturing have limited exposure margins and do not consistently produce high-quality resist patterns, necessitating improvements in both exposure tolerance and pattern shape.

Method used

A copolymer with a specific monomer unit having a calculated lowest unoccupied molecular orbital (LUMO) of -0.70 eV or more is used, which widens the exposure margin and enhances the shape of the resist pattern when exposed to ionizing radiation, combined with a solvent and development using an alcohol-based developer.

Benefits of technology

The copolymer and resist composition enable the formation of resist patterns with improved exposure margins and better shape retention, suitable for advanced semiconductor manufacturing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011498_03102024_PF_FP_ABST
    Figure JP2024011498_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide a copolymer and a positive resist composition, which make it possible to form a resist pattern that has a wide light exposure margin and a favorable shape. A copolymer according to the present invention is characterized by comprising a monomer unit (I) represented by formula (I) and a monomer unit (II) represented by formula (II). In the formulae, R1, R2, R3, R4, R5, R6, R7 and R8 each represent a specific group, and p represents an integer of 0 to 5 (inclusive).
Need to check novelty before this filing date? Find Prior Art

Description

Copolymer, positive resist composition, and method for forming a resist pattern

[0001] The present invention relates to a copolymer, a positive resist composition, and a method of forming a resist pattern.

[0002] Conventionally, in fields such as semiconductor manufacturing, polymers whose main chains are scissed and whose solubility in a developer is increased by irradiation with ionizing radiation such as electron beams and extreme ultraviolet (EUV) radiation, or non-ionizing radiation including short-wavelength light such as ultraviolet radiation (hereinafter, sometimes collectively referred to as "ionizing radiation, etc.") have been used as main-chain scission-type positive resists. Specifically, for example, Patent Document 1 discloses a main-chain scission-type positive resist capable of efficiently forming fine resist patterns with high resolution, which contains a copolymer having α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl units and 4-methyl-α-methylstyrene units or α-methylstyrene units and having a weight-average molecular weight of more than 100,000.

[0003] International Publication No. 2022 / 070928

[0004] In recent years, due to demands for higher integration of semiconductor integrated circuits, etc., main chain scission type positive resists are required to have a wide exposure margin (i.e., a wide tolerance for the amount of exposure in the exposure step). Main chain scission type positive resists are also required to have an excellent resist pattern shape formed through the exposure step and development treatment (development step) using a developer. However, the above-mentioned conventional positive resists have room for improvement in terms of widening the exposure margin while providing a good resist pattern shape.

[0005] Therefore, an object of the present invention is to provide a copolymer and a positive resist composition that are capable of forming a resist pattern with a wide exposure margin and a good shape, and also to provide a method of forming a resist pattern that is capable of forming a resist pattern with a wide exposure margin and a good shape.

[0006] The present inventors have conducted extensive research to achieve the above object, and have newly discovered that by using a copolymer containing a predetermined monomer unit having a calculated lowest unoccupied molecular orbital (LUMO) value equal to or greater than a predetermined value, it is possible to form a resist pattern having a good shape while widening the exposure margin of the resist, and have completed the present invention.

[0007] That is, the object of the present invention is to advantageously solve the above-mentioned problems, and the present invention provides [1] a compound represented by the following formula (I): (In formula (I), R 1 is a halogen atom or an alkyl group substituted with a halogen atom, and R 2 is an aliphatic group which may have a substituent (provided that when the aliphatic group is a bridged cyclic saturated hydrocarbon group, it has a substituent), and R 3 and R 4 are hydrogen atoms, halogen atoms, unsubstituted alkyl groups or alkyl groups substituted with halogen atoms, and may be the same or different from each other), and a monomer unit (I) represented by the following formula (II): (In formula (II), R 5 , R 7 and R 8 are hydrogen atoms, halogen atoms, unsubstituted alkyl groups or alkyl groups substituted with halogen atoms, and may be the same or different from each other; R 6 is a halogen atom or an organic group, and p is an integer of 0 or more and 5 or less. The copolymer comprises a monomer unit (II) represented by the formula: wherein the monomer unit (I) has a calculated lowest unoccupied molecular orbital (LUMO) of -0.70 eV or more. Thus, by using a copolymer containing a predetermined monomer unit (I) having a calculated lowest unoccupied molecular orbital (LUMO) of a predetermined value or more, it is possible to form a resist pattern having a good shape while widening the exposure margin of the resulting resist. In the present invention, the lowest unoccupied molecular orbital (LUMO) of the monomer unit (I) can be determined by the method described in the Examples.

[0008] [2] In the copolymer of [1] above, the R 2is preferably an aliphatic group having 1 to 20 carbon atoms which may have a substituent. 2 When is an aliphatic group having from 1 to 20 carbon atoms which may have a substituent, the exposure margin can be further widened and a resist pattern with an even better shape can be formed.

[0009] [3] In the copolymer of [1] or [2] above, the R 2 is preferably an aliphatic group having an electron-donating group as a substituent. 2 When is an aliphatic group having an electron-donating group as a substituent, it is possible to further widen the exposure margin and form a resist pattern with an even better shape.

[0010] Another object of the present invention is to advantageously solve the above-mentioned problems, and the present invention provides [4] a positive resist composition comprising the copolymer of any one of [1] to [3] above and a solvent. This positive resist composition makes it possible to form a resist pattern with an even better shape while further expanding the exposure margin.

[0011] Another object of the present invention is to advantageously solve the above-mentioned problems, and the present invention provides [5] a method of forming a resist pattern, comprising the steps of: forming a resist film using the positive resist composition according to the above [4]; exposing the resist film; and developing the exposed resist film. According to the above method of forming a resist pattern, a resist pattern having a good shape can be formed with a wide exposure margin.

[0012] [6] In the method for forming a resist pattern according to the above item [5], the development is preferably carried out using an alcohol-based solvent. By using an alcohol-based solvent for development, a resist pattern having a better shape can be formed.

[0013] According to the present invention, it is possible to provide a copolymer and a positive resist composition which are capable of forming a resist pattern which has a wide exposure margin and a good shape, and also to provide a method of forming a resist pattern which is capable of forming a resist pattern which has a wide exposure margin and a good shape.

[0014] Embodiments of the present invention are described in detail below. The copolymer of the present invention can be used, for example, to produce a main chain scission-type positive resist composition in which the main chain is scissed by ionizing radiation or the like, resulting in a lower molecular weight, and can be suitably used in the production of the positive resist composition of the present invention. The positive resist composition of the present invention comprises the copolymer of the present invention, and can be suitably used, for example, in the method of forming a resist pattern of the present invention. The method of forming a resist pattern of the present invention can be suitably used, for example, when forming a resist pattern in the production processes of printed circuit boards such as build-up boards, semiconductors, photomasks, molds, etc.

[0015] (Copolymer) The copolymer of the present invention is represented by the following formula (I): (In formula (I), R 1 is a halogen atom or an alkyl group substituted with a halogen atom, and R 2 is an aliphatic group which may have a substituent (provided that when the aliphatic group is a bridged cyclic saturated hydrocarbon group, it has a substituent), and R 3 and R 4 are hydrogen atoms, halogen atoms, unsubstituted alkyl groups or alkyl groups substituted with halogen atoms, and may be the same or different from each other.) and a monomer unit (I) represented by the following formula (II): (In formula (II), R 5 , R 7 and R 8 are hydrogen atoms, halogen atoms, unsubstituted alkyl groups or alkyl groups substituted with halogen atoms, and may be the same or different from each other; R 6is a halogen atom or an organic group, and p is an integer of 0 or more and 5 or less.) and a monomer unit (II) represented by the following formula:

[0016] The copolymer of the present invention may contain other monomer units besides the monomer unit (I) and the monomer unit (II), but the proportion of the monomer unit (I) and the monomer unit (II) in total of the monomer units (100 mol%) constituting the copolymer is preferably 70 mol% or more, more preferably 100 mol% (i.e., the copolymer consists of the monomer unit (I) and the monomer unit (II)). Furthermore, the copolymer of the present invention is not particularly limited as long as it contains the monomer unit (I) and the monomer unit (II), and may be either a random copolymer, a block copolymer, or the like.

[0017] The copolymer of the present invention contains the monomer unit (I) and the monomer unit (II), and when irradiated with ionizing radiation or the like, the main chain of the copolymer is effectively cleaved only in the irradiated portion, resulting in a low molecular weight. The low-molecular weight component is then well soluble in a developer. The reason why the calculated lowest unoccupied molecular orbital (LUMO) of the monomer unit (I) in the copolymer of the present invention widens the exposure margin of the resulting resist and allows for the formation of a good resist pattern shape is not entirely clear, but is presumed to be as follows. That is, when the calculated lowest unoccupied molecular orbital (LUMO) of the monomer unit (I) is -0.70 eV or more, the tolerance for receiving high energy, such as ionizing radiation, is increased, making the copolymer more susceptible to receiving high energy, and as a result, the main chain of the copolymer is effectively cleaved upon irradiation with ionizing radiation or the like.

[0018] From the viewpoint of further widening the exposure margin and forming a resist pattern having a better shape, the calculated value of the lowest unoccupied molecular orbital (LUMO) of the monomer unit (I) is preferably −0.50 eV or more, and more preferably −0.20 eV or more.

[0019] <Monomer Unit (I)> The monomer unit (I) contained in the copolymer of the present invention is a monomer unit represented by the following formula (a): (In formula (a), R 1 ~R 4 has the same meaning as formula (I).

[0020] Here, R in formula (I) and formula (a) 1 , R 3 , R 4 The halogen atom that can constitute the monomer unit (I) is not particularly limited as long as the calculated value of the lowest unoccupied molecular orbital (LUMO) of the monomer unit (I) is −0.70 eV or more, and examples thereof include a chlorine atom, a fluorine atom, a bromine atom, and an iodine atom. 1 , R 3 , R 4 The alkyl group substituted with a halogen atom that can constitute the above formula (I) is not particularly limited as long as the calculated value of the lowest unoccupied molecular orbital (LUMO) of the monomer unit (I) is −0.70 eV or more, and examples thereof include groups having a structure in which some or all of the hydrogen atoms in the alkyl group are substituted with the above halogen atoms. 3 , R 4 The unsubstituted alkyl group that can constitute R is not particularly limited as long as the calculated value of the lowest unoccupied molecular orbital (LUMO) of the monomer unit (I) is −0.70 eV or more, and examples thereof include unsubstituted alkyl groups having 1 to 10 carbon atoms. 3 , R 4 The unsubstituted alkyl group that can constitute the above is preferably a methyl group or an ethyl group.

[0021] From the viewpoint of improving the scission property of the main chain of the copolymer when irradiated with exposure light and increasing the efficiency of forming a resist pattern, R 1 is preferably a chlorine atom, a fluorine atom, or an alkyl group having 1 to 5 carbon atoms substituted with a fluorine atom, more preferably a chlorine atom, a fluorine atom, or a perfluoromethyl group, further preferably a chlorine atom or a fluorine atom, and particularly preferably a chlorine atom. 1The monomer (a) in which R is a chlorine atom has excellent polymerizability, and 1 The copolymer having the monomer unit (I) in which is a chlorine atom is also advantageous in that it can be easily prepared.

[0022] Furthermore, from the viewpoint of improving the scission property of the polymer main chain when irradiated with exposure light and increasing the efficiency of resist pattern formation, it is preferable that R 3 and R 4 are each preferably a hydrogen atom or an unsubstituted alkyl group, more preferably a hydrogen atom or an unsubstituted alkyl group having 1 to 5 carbon atoms, and even more preferably a hydrogen atom.

[0023] R in formula (I) and formula (a) 2 The "optionally substituted aliphatic group (provided that when the aliphatic group is a bridged cyclic saturated hydrocarbon group, it has a substituent)" that can constitute R is not particularly limited, as long as the calculated value of the lowest unoccupied molecular orbital (LUMO) of the monomer unit (I) is -0.70 eV or more. From the viewpoint of further widening the exposure margin and forming a resist pattern with a better shape, R 2 is preferably an aliphatic group having 1 to 20 carbon atoms which may have a substituent, more preferably an aliphatic group having 1 to 12 carbon atoms which may have a substituent, and even more preferably an aliphatic group having 1 to 10 carbon atoms which may have a substituent. The above "number of carbon atoms" means the number of carbon atoms in the aliphatic group, not including the number of carbon atoms in the substituent. Examples of the aliphatic group include chain aliphatic groups and cyclic aliphatic groups.

[0024] Examples of the chain aliphatic group include, but are not limited to, an alkyl group, an alkenyl group, and the like. Examples of the alkyl group include, but are not limited to, an alkyl group having from 1 to 20 carbon atoms, specifically, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a tert-butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, and a decyl group. Of these, an isopropyl group and a tert-butyl group are preferred. Examples of the alkenyl group include, but are not limited to, an alkenyl group having from 1 to 20 carbon atoms, specifically, an ethenyl group (vinyl group), a propenyl group, an isopropenyl group, a butenyl group, an isobutenyl group, a tert-butenyl group, a pentenyl group, a hexenyl group, a heptenyl group, an octenyl group, an isooctenyl group, and a nonenyl group.

[0025] The cyclic aliphatic group may be either monocyclic or polycyclic, and examples of monocyclic cyclic aliphatic groups include cycloalkyl groups and cycloalkenyl groups. The cycloalkyl group is not particularly limited, and examples thereof include cycloalkyl groups having from 3 to 20 carbon atoms, specific examples of which include cyclopropyl groups, cyclobutyl groups, cyclopentyl groups, cyclohexyl groups, cyclooctyl groups, cyclononyl groups, and cyclodecyl groups. Of these, cyclohexyl groups are preferred. The cycloalkenyl group is not particularly limited, and examples thereof include cycloalkenyl groups having from 3 to 20 carbon atoms, specific examples of which include 1-cyclopropyl groups, 1-cyclobutenyl groups, 1-cyclopentenyl groups, 1-cyclohexenyl groups, 1-cycloheptenyl groups, and 1-cyclooctenyl groups.

[0026] The polycyclic alicyclic group is not particularly limited, and examples thereof include bridged cyclic saturated hydrocarbon groups such as norbornyl and adamantyl groups. Of these, an adamantyl group is preferred. The bridged cyclic saturated hydrocarbon group refers to a group having a ring structure with one or more bridge groups (e.g., alkylene groups such as methylene groups) connecting two or more non-adjacent carbon atoms of a saturated hydrocarbon ring.

[0027] The substituent is not particularly limited as long as the calculated lowest unoccupied molecular orbital (LUMO) of the monomer unit (I) is -0.70 eV or greater, and examples thereof include halogen atoms such as chlorine atoms, fluorine atoms, bromine atoms, and iodine atoms, hydroxyl groups, alkyl groups, cycloalkyl groups, alkylamino groups, dialkylamino groups, and alkoxy groups. These alkyl groups, cycloalkyl groups, alkylamino groups, dialkylamino groups, and alkoxy groups may be further substituted with the halogen atoms or hydroxyl groups. When multiple substituents are present, the multiple substituents may be the same or different from each other.

[0028] The alkyl group as the substituent is not particularly limited, and R 2 Among these, alkyl groups having 1 to 4 carbon atoms, specifically, methyl, ethyl, n-propyl, isopropyl, isobutyl, and tert-butyl groups are preferred.

[0029] The cycloalkyl group as the substituent is not particularly limited, and R 2 Among these, a cycloalkyl group having 3 to 10 carbon atoms, such as a cyclohexyl group, is preferred.

[0030] Examples of the alkoxy group as the substituent include alkoxy groups having 1 to 12 carbon atoms, such as methoxy, ethoxy, and butoxy groups. Of these, methoxy is preferred.

[0031] Examples of the alkylamino group as the substituent include alkylamino groups having 1 to 12 carbon atoms, such as a methylamino group, an ethylamino group, an n-propylamino group, an i-propylamino group, a cyclopropylamino group, an n-butylamino group, an i-butylamino group, an s-butylamino group, a t-butylamino group, and a cyclobutylamino group.

[0032] Examples of the dialkylamino group as the substituent include dialkylamino groups having 2 to 12 carbon atoms, such as dimethylamino, diethylamino, dipropylamino, and dibutylamino.

[0033] Among these, from the viewpoint of forming a resist pattern having a better shape while further widening the exposure margin, the substituent is preferably an electron-donating group. Preferred electron-donating groups include a hydroxyl group, as well as the above-mentioned alkyl group, cycloalkyl group, alkoxy group (when substituted at the aryl position of an alkenyl group or the like), alkylamino group, and dialkylamino group, with a hydroxyl group or an alkyl group being more preferred.

[0034] As described above, when the aliphatic group is a bridged cyclic saturated hydrocarbon group, the bridged cyclic saturated hydrocarbon group needs to have a substituent. By having the bridged cyclic saturated hydrocarbon group have a substituent, the exposure margin can be widened and a resist pattern with a good shape can be formed. Here, among the above-mentioned substituents, the substituent that the bridged cyclic saturated hydrocarbon group has is preferably an alkoxy group or a hydroxyl group, and more preferably a hydroxyl group.

[0035] The monomer (a) represented by the above formula (a) capable of forming the monomer unit (I) represented by the above formula (I) having a calculated low-vacant molecular orbital (LUMO) of −0.70 eV or more is not particularly limited, and examples thereof include isopropyl α-chloroacrylate, t-butyl α-chloroacrylate, cyclohexyl α-chloroacrylate, 4-t-butylcyclohexyl α-chloroacrylate, 4-methylcyclohexyl α-chloroacrylate, 4-hydroxycyclohexyl α-chloroacrylate, and 3,4-dimethylcyclohexyl α-chloroacrylate. Examples of chloroacrylates include cyclohexyl α-chloroacrylate, 3,3,5-trimethylcyclohexyl α-chloroacrylate, 4-methoxycyclohexyl α-chloroacrylate, 4-isopropylcyclohexyl α-chloroacrylate, 4-ethylcyclohexyl α-chloroacrylate, cycloheptyl α-chloroacrylate, cyclooctyl α-chloroacrylate, bicyclohexyl α-chloroacrylate, 3-hydroxyadamantyl α-chloroacrylate, 3,7-dihydroxyadamantyl α-chloroacrylate, and 3-methoxyadamantyl α-chloroacrylate. These may be used alone or in combination of two or more. Among these, 4-t-butylcyclohexyl α-chloroacrylate, 4-methylcyclohexyl α-chloroacrylate, isopropyl α-chloroacrylate, and 3-hydroxyadamantyl α-chloroacrylate are preferred, with 4-t-butylcyclohexyl α-chloroacrylate being more preferred.

[0036] That is, examples of the monomer unit (I) represented by the above formula (I) having a calculated unoccupied orbital LUMO of −0.70 eV or more include monomer units represented by the following (a-1) to (a-19):

[0037] Among these, the monomer unit (I) is a monomer unit represented by (a-1) (i.e., in formula (I), R 1 is a chlorine atom, and R 3 and R 4 is a hydrogen atom, and R 2is a 4-t-butylcyclohexyl group), a monomer unit represented by (a-2) (i.e., a monomer unit represented by (a-3) in formula (I), 1 is a chlorine atom, and R 3 and R 4 is a hydrogen atom, and R 2 is a 4-methylcyclohexyl group), a monomer unit represented by (a-3) (i.e., a monomer unit represented by (a-4) in formula (I), 1 is a chlorine atom, and R 3 and R 4 is a hydrogen atom, and R 2 is an isopropyl group), a monomer unit represented by (a-4) (i.e., a monomer unit represented by (a-5) in formula (I), 1 is a chlorine atom, and R 3 and R 4 is a hydrogen atom, and R 2 a monomer unit represented by (a-18) (i.e., a monomer unit represented by (a-19) in which R 1 is a chlorine atom, and R 3 and R 4 is a hydrogen atom, and R 2 is a 2,2,3,3-tetrafluoropropyl group), and a monomer unit represented by (a-19) (i.e., a monomer unit represented by (a-20) in formula (I), 1 is a chlorine atom, and R 3 and R 4 is a hydrogen atom, and R 2 is a 2,2,3,4,4,4-hexafluorobutyl group), and the monomer unit represented by (a-1) is more preferred. Specific calculated values ​​of the unoccupied orbital LUMO of the monomer units (I) represented by (a-1) to (a-19) above are shown in Table 1 below.

[0038] The proportion of the monomer units (I) in the copolymer is preferably 20 mol% or more, more preferably 30 mol% or more, and even more preferably 40 mol% or more, and preferably 80 mol% or less, more preferably 75 mol% or less, and even more preferably 70 mol% or less, when the total amount of all the monomer units in the copolymer is taken as 100 mol%. If the proportion of the monomer units (I) in the copolymer is within the above range, when the total amount of all the monomer units in the copolymer is taken as 100 mol%, it is possible to form a resist pattern having a better shape while further widening the exposure margin.

[0039] <Monomer Unit (II)> The monomer unit (II) contained in the copolymer of the present invention is a monomer unit represented by the following formula (b): (In formula (b), R 5 ~R 8 is a structural unit derived from a monomer (b) represented by formula (II).

[0040] R in formula (II) and formula (b) 5 , R 7 , R 8 The halogen atom or alkyl group substituted with a halogen atom that can constitute the formula (II) or (b) includes, but is not limited to, halogen atoms such as chlorine, fluorine, bromine, and iodine atoms; and groups having a structure in which some or all of the hydrogen atoms in the alkyl group are substituted with the above-mentioned halogen atoms. 5 , R 7 , R 8 The unsubstituted alkyl group that can constitute R is not particularly limited, and examples thereof include unsubstituted alkyl groups having 1 to 5 carbon atoms. 5 , R 7 , R 8 The unsubstituted alkyl group that can constitute the above is preferably a methyl group or an ethyl group.

[0041] R in formula (II) and formula (b) 6 The halogen atom that can constitute the group is not particularly limited, and examples thereof include a chlorine atom, a fluorine atom, a bromine atom, an iodine atom, etc. Among these, a fluorine atom is preferred.

[0042] In addition, R in formula (II) and formula (b) 6 Examples of organic groups that can constitute R include unsubstituted alkyl groups, alkyl groups substituted with halogen atoms, alkoxy groups, and alkoxy groups substituted with halogen atoms. 6 The unsubstituted alkyl group that can constitute R is not particularly limited, and examples thereof include unsubstituted alkyl groups having 1 to 10 carbon atoms. The alkyl group may be either linear or cyclic. Among these, a methyl group, an ethyl group, an isopropyl group, a cyclohexyl group, or an adamantyl group is preferred. 6 The alkyl group substituted with a halogen atom that can constitute R is not particularly limited, and examples thereof include groups having a structure in which some or all of the hydrogen atoms in the alkyl group have been substituted with the above-mentioned halogen atoms. 6 The alkoxy group that can constitute R is not particularly limited, and examples thereof include alkoxy groups having 1 to 5 carbon atoms. Among these, a methoxy group or an ethoxy group is preferred. 6 The alkoxy group substituted with a halogen atom that can constitute the above group is not particularly limited, and examples thereof include groups having a structure in which some or all of the hydrogen atoms in the alkoxy group have been substituted with the above halogen atoms.

[0043] In addition, R 6 When there are a plurality of R (i.e., when p is an integer of 2 or more and 5 or less), 6 may be the same or different from each other.

[0044] Examples of the monomer (b) represented by the above formula (b) which can form the monomer unit (II) represented by the above formula (II) include α-methylstyrene (AMS) and its derivatives such as the following (b-1) to (b-20).

[0045] From the viewpoint of improving the ease of preparation of the copolymer, the monomer unit (II) preferably does not contain a fluorine atom, and is more preferably a structural unit derived from α-methylstyrene. 5is a methyl group, p=0, and R 7 and R 8 is preferably a hydrogen atom.

[0046] The proportion of the monomer unit (II) in the copolymer is not particularly limited, and is preferably 20 mol% or more, more preferably 30 mol% or more, and even more preferably 40 mol% or more, when the total amount of all monomer units in the copolymer is 100 mol%, and is preferably 80 mol% or less, more preferably 75 mol% or less, and even more preferably 70 mol% or less.

[0047] <Properties of the Copolymer> [Weight-Average Molecular Weight (Mw)] The weight-average molecular weight (Mw) of the copolymer is preferably 10,000 or more, more preferably 20,000 or more, even more preferably 30,000 or more, and preferably 500,000 or less, more preferably 400,000 or less, and even more preferably 350,000 or less. If the weight-average molecular weight (Mw) of the copolymer is equal to or greater than the above-mentioned lower limit, excessive increase in the solubility of the resist film in the developer can be suppressed even at a low irradiation dose, and a resist pattern with a better shape can be formed. On the other hand, if the weight-average molecular weight (Mw) of the copolymer is equal to or less than the above-mentioned upper limit, a positive resist composition can be easily prepared. In this specification, the "weight-average molecular weight" can be measured by the method described in the Examples.

[0048] [Number Average Molecular Weight (Mn)] The number average molecular weight (Mn) of the copolymer is preferably 5,000 or more, more preferably 10,000 or more, and even more preferably 12,000 or more, and preferably 400,000 or less, more preferably 350,000 or less, even more preferably 300,000 or less, and even more preferably 250,000 or less. If the number average molecular weight of the copolymer is equal to or greater than the above lower limit, excessive increase in the solubility of the resist film in the developer at a low irradiation dose can be further suppressed, and a resist pattern with a better shape can be formed. On the other hand, if the number average molecular weight of the copolymer is equal to or less than the above upper limit, a positive resist composition can be more easily prepared. In this specification, the "number average molecular weight" can be measured by the method described in the Examples.

[0049] [Molecular Weight Distribution (Mw / Mn)] The molecular weight distribution (Mw / Mn) of the copolymer is preferably 1.10 or more, more preferably 1.20 or more, even more preferably 1.50 or more, and preferably 2.20 or less, more preferably 2.00 or less, and even more preferably 1.95 or less. If the molecular weight distribution (Mw / Mn) of the copolymer is equal to or greater than the lower limit, the ease of production of the copolymer can be improved. On the other hand, if the molecular weight distribution (Mw / Mn) of the copolymer is equal to or less than the upper limit, the shape of the obtained resist pattern can be further improved. In this specification, the "molecular weight distribution" can be determined by calculating the ratio of the weight average molecular weight to the number average molecular weight (weight average molecular weight / number average molecular weight).

[0050] <Method for Preparing Copolymer> The method for preparing the copolymer is not particularly limited. For example, a copolymer containing monomer unit (I) and monomer unit (II) can be prepared by polymerizing a monomer composition containing monomer (a), monomer (b), and any monomer copolymerizable with these monomers, recovering the resulting copolymer, and optionally purifying it. The composition, molecular weight distribution, number average molecular weight, and weight average molecular weight of the copolymer can be adjusted by changing the polymerization conditions and purification conditions. Specifically, for example, the number average molecular weight and weight average molecular weight can be increased by lowering the polymerization temperature. Furthermore, the number average molecular weight and weight average molecular weight can be increased by shortening the polymerization time. Furthermore, purification can narrow the molecular weight distribution.

[0051] [Polymerization of Monomer Composition] The monomer composition used to prepare the copolymer may be, for example, a mixture of monomer components containing monomer (a), monomer (b), and any monomer copolymerizable with these monomers, an optionally usable solvent, an optionally usable polymerization initiator, and any additives. Polymerization of the monomer composition can be carried out using known methods. Among these, cyclopentanone, water, or the like is preferably used as the solvent. Furthermore, azobisisobutyronitrile, dimethyl 2,2'-azobis(2-methylpropionate), or the like is preferably used as the polymerization initiator.

[0052] The polymer obtained by polymerizing the monomer composition can be recovered by adding a good solvent such as tetrahydrofuran to a solution containing the polymer, and then dropping the solution to which the good solvent has been added into a poor solvent such as methanol, ethanol, 1-propanol, 1-butanol, 1-pentanol, or hexane to coagulate the polymer, without any particular limitation.

[0053] [Purification of Polymer] The purification method used to purify the obtained polymer is not particularly limited, and known purification methods such as reprecipitation and column chromatography can be used. Among them, the reprecipitation method is preferred as the purification method. The purification of the polymer may be repeated multiple times.

[0054] Purification of a polymer by the reprecipitation method is preferably carried out, for example, by dissolving the obtained polymer in a good solvent such as tetrahydrofuran, and then dropping the resulting solution into a mixed solvent of a good solvent such as tetrahydrofuran and a poor solvent such as methanol, ethanol, 1-propanol, 1-butanol, 1-pentanol, or hexane to precipitate a portion of the polymer. In this way, by dropping a solution of the polymer into a mixed solvent of a good solvent and a poor solvent to perform purification, the molecular weight distribution, number average molecular weight, and weight average molecular weight of the resulting copolymer can be easily adjusted by changing the type and mixing ratio of the good solvent and poor solvent. Specifically, for example, the molecular weight of the copolymer precipitated in the mixed solvent can be increased by increasing the proportion of the good solvent in the mixed solvent.

[0055] When purifying a polymer by the reprecipitation method, a polymer precipitated in a mixed solvent of a good solvent and a poor solvent may be used as the copolymer, as long as the copolymer has the desired properties. Alternatively, a polymer not precipitated in the mixed solvent (i.e., a polymer dissolved in the mixed solvent) may be used. Here, the polymer not precipitated in the mixed solvent can be recovered from the mixed solvent by a known method such as concentration to dryness.

[0056] (Positive Resist Composition) The positive resist composition of the present invention comprises the copolymer of the present invention and a solvent. Because the positive resist composition of the present invention contains the above-mentioned copolymer of the present invention, it is possible to form a resist pattern with a good shape while widening the exposure margin of the resulting resist.

[0057] <Copolymer> As the copolymer, the copolymer of the present invention described above can be used.

[0058] When the total of all components of the positive resist composition is taken as 100 mass %, the content of the copolymer in the positive resist composition is preferably 0.5 mass % or more, more preferably 1 mass % or more, and even more preferably 1.5 mass % or more, and is preferably 15 mass % or less, more preferably 10 mass % or less, and even more preferably 5 mass % or less.

[0059] <Solvent> There are no particular restrictions on the solvent, as long as it is capable of dissolving the copolymer of the present invention, and it is possible to use known solvents such as those described in Japanese Patent No. 5938536. Among these, from the perspective of obtaining a positive resist composition with an appropriate viscosity and improving the coatability of the positive resist composition, it is preferable to use anisole, propylene glycol monomethyl ether acetate (PGMEA), cyclopentanone, cyclohexanone, or isoamyl acetate as the solvent, and it is more preferable to use isoamyl acetate.

[0060] <Other Components> In addition to the components described above, the positive resist composition of the present invention may optionally further contain known additives that can be incorporated into resist compositions. There are no particular restrictions on the amount of additives that can be incorporated, and an appropriate amount can be added depending on the application.

[0061] <Preparation of Positive Resist Composition> The positive resist composition can be prepared by mixing the copolymer of the present invention, a solvent, and any known additives that can be used. There are no particular limitations on the mixing method, and mixing can be carried out using a known method. Alternatively, the resist composition can be prepared by mixing the components and then filtering the mixture.

[0062] [Filtration] The method for filtering the mixture is not particularly limited, and can be, for example, a filter. The filter is not particularly limited, and examples include fluorocarbon, cellulose, nylon, polyester, and hydrocarbon-based filter membranes. Among these, from the viewpoint of effectively preventing impurities such as metals from being mixed into the positive resist composition from metal piping, etc., which may be used during the preparation of the copolymer of the present invention, preferred filter materials include polyfluorocarbons such as polyethylene, polypropylene, polytetrafluoroethylene, and Teflon (registered trademark), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymers (PFA), nylon, and composite membranes of polyethylene and nylon. Filters such as those disclosed in U.S. Pat. No. 6,103,122 may be used. Alternatively, commercially available filters such as Zeta Plus (registered trademark) 40Q manufactured by CUNO Incorporated may be used. Furthermore, the filter may contain a strong or weak cationic ion exchange resin. The average particle size of the ion exchange resin is not particularly limited, but is preferably 2 μm or more and 10 μm or less. Examples of cation exchange resins include sulfonated phenol-formaldehyde condensates, sulfonated phenol-benzaldehyde condensates, sulfonated styrene-divinylbenzene copolymers, sulfonated methacrylic acid-divinylbenzene copolymers, and other types of sulfonic or carboxylic acid group-containing polymers. + Counterion, NH 4 + counterion or alkali metal counterion, e.g., K + and Na + Counterions are provided. The cation exchange resin preferably has hydrogen counterions. Examples of such cation exchange resins include H +Sulfonated styrene-divinylbenzene copolymers with counterions, such as Microlite® PrCH from Purolite Corp. Such cation exchange resins are commercially available as AMBERLYST® from Rohm and Haas.

[0063] The pore size of the filter is preferably from 0.001 μm to 1 μm, inclusive. If the pore size of the filter is within this range, it is possible to sufficiently prevent impurities such as metals from being mixed into the positive resist composition.

[0064] (Method of Forming Resist Pattern) The method of forming a resist pattern of the present invention includes at least the steps of forming a resist film using the above-described positive resist composition of the present invention (resist film formation step), exposing the resist film (exposure step), and developing the exposed resist film (development step). Furthermore, the method of forming a resist pattern of the present invention may also include, for example, a step of forming an underlayer film on the substrate on which the resist film will be formed (underlayer film formation step) prior to the resist film formation step. The method of forming a resist pattern of the present invention may also include a step of heating the resist film between the exposure step and the development step (post-exposure bake (PEB) step), and / or a step of removing the developer after the development step (developer removal step). After forming a resist pattern by the method of forming a resist pattern, the method of forming a resist pattern of the present invention may also include a step of etching the underlayer film and / or the substrate (etching step). Because the method of forming a resist pattern of the present invention uses the positive resist composition of the present invention as the positive resist composition, a resist pattern with a good shape can be formed with a wide exposure margin.

[0065] <Underlayer Film Formation Step> In the underlayer film formation step, which can be optionally performed before the resist film formation step, an underlayer film is formed on a substrate. By providing the underlayer film on the substrate, the surface of the substrate is made hydrophobic. This increases the affinity between the substrate and the resist film, thereby improving the adhesion between the substrate and the resist film. The underlayer film may be an inorganic underlayer film or an organic underlayer film.

[0066] The inorganic underlayer film can be formed by applying an inorganic material onto a substrate and then baking it, etc. Examples of inorganic materials include silicon-based materials.

[0067] The organic underlayer film can be formed by applying an organic material to a substrate to form a coating film and drying it. The organic material is not limited to those sensitive to light or electron beams, and can include, for example, resist materials and resin materials commonly used in the semiconductor and liquid crystal fields. Among these, the organic material is preferably a material capable of forming an organic underlayer film that can be etched, particularly dry etched. With such an organic material, the organic underlayer film can be etched using a pattern formed by processing a resist film, thereby transferring the pattern to the underlayer film and forming a pattern in the underlayer film. Among these, the organic material is preferably a material capable of forming an organic underlayer film that can be etched by oxygen plasma etching or the like. Examples of organic materials used to form the organic underlayer film include AL412 from Brewer Science.

[0068] The organic material can be applied by a conventional method using spin coating or a spinner. The method for drying the coating film can be any method capable of volatilizing the solvent contained in the organic material, such as baking. The baking conditions are not particularly limited, but the baking temperature is preferably 80°C or higher and 300°C or lower, and more preferably 200°C or higher and 300°C or lower. The baking time is preferably 30 seconds or longer, more preferably 60 seconds or longer, and preferably 500 seconds or shorter, more preferably 400 seconds or shorter, even more preferably 300 seconds or shorter, and particularly preferably 180 seconds or shorter. The thickness of the underlayer film after drying the coating film is not particularly limited, but is preferably 10 nm or higher and 100 nm or lower.

[0069] [Substrate] Here, the substrate on which the underlayer film or resist film can be formed in the resist pattern forming method is not particularly limited, and examples that can be used include a substrate having an insulating layer and copper foil provided on the insulating layer, which is used in the manufacture of printed circuit boards, etc.; and a mask blank having a light-shielding layer formed on a substrate.

[0070] The substrate material may be, for example, metal (silicon, copper, chromium, iron, aluminum, etc.), glass, titanium oxide, silicon dioxide (SiO 2 Examples of suitable substrates include inorganic materials such as silica and mica; nitrides such as SiN; oxynitrides such as SiON; and organic materials such as acrylic, polystyrene, cellulose, cellulose acetate, and phenolic resin. Among these, metals are preferred as the substrate material. By using, for example, a silicon substrate, a silicon dioxide substrate, or a copper substrate, preferably a silicon substrate or a silicon dioxide substrate, as the substrate, a cylindrical structure can be formed.

[0071] The size and shape of the substrate are not particularly limited. The surface of the substrate may be smooth, curved, or uneven, and may be a thin plate-shaped substrate.

[0072] The surface of the substrate may be subjected to a surface treatment as necessary. For example, in the case of a substrate having hydroxyl groups on its surface layer, the surface of the substrate can be treated using a silane coupling agent capable of reacting with the hydroxyl groups. This changes the surface layer of the substrate from hydrophilic to hydrophobic, thereby improving the adhesion between the substrate and the underlayer film or between the substrate and the resist layer. In this case, the silane coupling agent is not particularly limited, but hexamethyldisilazane is preferred.

[0073] <Resist film forming step> In the resist film forming step, the positive resist composition of the present invention is applied onto a workpiece such as a substrate to be processed using the resist pattern (or onto an underlayer film if an underlayer film has been formed) to obtain a coating layer (coating step), and then the solvent is removed from the obtained coating layer to form a resist film (drying step).

[0074] [Coating Step] The workpiece to be coated with the positive resist composition of the present invention in the coating step is not particularly limited, and examples that can be used include semiconductor substrates used in the manufacture of semiconductor devices, etc.; substrates having an insulating layer and copper foil provided on the insulating layer, used in the manufacture of printed circuit boards, etc.; and mask blanks having a light-shielding layer formed on a substrate. Furthermore, there are no particular limitations on the method for coating the positive resist composition of the present invention, and any known method can be used.

[0075] [Drying Step] The method for removing the solvent from the coating layer is not particularly limited, and a drying method commonly used in forming a resist film can be used. However, it is preferable to form a resist film by heating (prebaking) the positive resist composition. Here, the temperature at which the coating layer is dried (drying temperature) is preferably 100°C or higher, more preferably 110°C or higher, from the viewpoint of adhesion between the resist film formed through the drying step and the workpiece. Furthermore, from the viewpoint of reducing the thermal influence on the workpiece and the resist film, it is preferably 250°C or lower, more preferably 200°C or lower. The time for drying the coating layer (drying time) is preferably more than 10 seconds, more preferably 30 seconds or higher, even more preferably 1 minute or higher, from the viewpoint of sufficiently improving adhesion between the resist film formed by performing the drying step at a lower temperature range and the workpiece. From the viewpoint of reducing the change in molecular weight of the polymer in the resist film before and after the drying step, it is preferably 60 minutes or lower, more preferably 30 minutes or lower.

[0076] <Exposure Step> In the exposure step, the resist film formed in the resist film formation step is irradiated with ionizing radiation or the like to write a desired pattern. For electron beam irradiation, known writing devices such as electron beam writing devices and EUV exposure devices can be used. Here, ionizing radiation is radiation that has sufficient energy to ionize atoms or molecules. In contrast, non-ionizing radiation is radiation that does not have sufficient energy to ionize atoms or molecules.

[0077] Examples of ionizing radiation include electron beams, extreme ultraviolet rays, gamma rays, X-rays, alpha rays, heavy particle beams, proton beams, beta rays, and ion beams. Among these, electron beams or extreme ultraviolet rays are preferred as ionizing radiation, and electron beams are more preferred. The wavelength of extreme ultraviolet rays is not particularly limited, and can be, for example, 1 nm or more and 30 nm or less, and preferably 13.5 nm.

[0078] The nonionizing radiation is not particularly limited, but it is preferable to use nonionizing radiation having a wavelength of 300 nm or less. Examples of nonionizing radiation having a wavelength of 300 nm or less include far ultraviolet radiation excluding extreme ultraviolet radiation (wavelength: 40 nm or more and 200 nm or less) and near ultraviolet radiation (wavelength: more than 200 nm and 300 nm or less). Among these, KrF excimer laser radiation (wavelength: 248 nm) and ArF excimer laser radiation (wavelength: 193 nm) are preferred.

[0079] <Post-exposure bake step> In the post-exposure bake step, which may be optionally performed, the resist film exposed in the exposure step is heated. By performing the post-exposure bake step, the surface roughness of the resist pattern can be reduced.

[0080] Here, the heating temperature is preferably 70° C. or higher, more preferably 80° C. or higher, and even more preferably 90° C. or higher, and is preferably 200° C. or lower, more preferably 170° C. or lower, and even more preferably 150° C. or lower. When the heating temperature is within the above range, the clarity of the resist pattern can be improved while the surface roughness of the resist pattern can be effectively reduced.

[0081] The time for heating the resist film in the post-exposure bake step (heating time) is preferably 10 seconds or longer, more preferably 20 seconds or longer, and even more preferably 30 seconds or longer. A heating time of 10 seconds or longer can further improve the clarity of the resist pattern while sufficiently reducing the surface roughness of the resist pattern. On the other hand, from the viewpoint of production efficiency, the heating time is, for example, preferably 10 minutes or shorter, more preferably 5 minutes or shorter, and even more preferably 3 minutes or shorter.

[0082] The method for heating the resist film in the post-exposure bake step is not particularly limited, and examples thereof include a method of heating the resist film on a hot plate, a method of heating the resist film in an oven, and a method of blowing hot air onto the resist film.

[0083] <Developing Step> In the developing step, the exposed resist film (or the exposed and heated resist film if a post-exposure bake step has been performed) is developed to form a developed film on the workpiece. Here, the resist film can be developed, for example, by contacting the resist film with a developer. The method for contacting the resist film with the developer is not particularly limited, and known methods such as immersing the resist film in the developer or applying the developer to the resist film can be used.

[0084] [Developer] The developer can be appropriately selected depending on the properties of the copolymer of the present invention. Specifically, when selecting a developer, it is preferable to select a developer that does not dissolve the resist film before the exposure step, but can dissolve the exposed portion of the resist film after the exposure step. One type of developer may be used alone, or two or more types may be mixed in any ratio. As the developer, for example, 1,1,1,2,3,4,4,5,5,5-decafluoropentane (CF 3 CFHCFHCF 2 CF 3 ), 1,1,1,2,2,3,3,4,4,5,5,6,6-tridecafluorohexane, 1,1,1,2,2,3,4,5,5,5-decafluoropentane, 1,1,1,3,3-pentafluorobutane, 1,1,1,2,2,3,3,4,4-nonafluorohexane, and other hydrofluorocarbons; 2,2-dichloro-1,1,1-trifluoroethane, 1,1-dichloro-1-fluoroethane, 1,1-dichloro-2,2,3,3,3-pentafluoropropane (CF 3 CF 2 CHCl 2 ), 1,3-dichloro-1,1,2,2,3-pentafluoropropane (CClF 2 CF 2CHClF), methyl nonafluorobutyl ether (CF 3 CF 2 CF 2 CF 2 OCH 3 ), methyl nonafluoroisobutyl ether, ethyl nonafluorobutyl ether (CF 3 CF 2 CF 2 CF 2 O.C. 2 H 5 ), ethyl nonafluoroisobutyl ether, perfluorohexyl methyl ether (CF 3 CF 2 CF (OCH 3 ) C 3 F 7 ) and hydrofluoroethers such as CF 4 , C 2 F 6 , C 3 F 8 , C 4 F 8 , C 4 F 10 , C 5 F 12 , C 6 F 12 , C 6 F 14 , C 7 F 14 , C 7 F 16 , C 8 F 18 , C 9 F 20Examples of suitable developers that can be used include perfluorocarbons such as fluorine-based solvents, perfluorocarbons such as ethanol, 1-propanol, 2-propanol (isopropyl alcohol), 1-butanol, 2-butanol, 1-pentanol, 2-pentanol, and 3-pentanol; alkyl acetate solvents such as amyl acetate and hexyl acetate; mixtures of fluorine-based solvents and alcohol-based solvents; mixtures of fluorine-based solvents and alkyl acetate solvents; mixtures of alcohol-based solvents and alkyl acetate solvents; and mixtures of fluorine-based solvents, alcohol-based solvents, and alkyl acetate solvents. Among these, from the viewpoint of imparting a better shape to the resist pattern, it is preferable to use an alcohol-based solvent as the developer, and it is more preferable to use isopropyl alcohol.

[0085] <Developer Removal Step> In the developer removal step optionally included in the resist pattern formation method, the developer is removed from the developed resist film to form a resist pattern on the workpiece. The developer can be removed by air blowing using a gas such as nitrogen, or by rinsing using a rinse solution. Here, the method for contacting the developed resist film with the rinse solution in the rinse process is not particularly limited, and known methods such as immersing the resist film in the rinse solution or applying the rinse solution to the resist film can be used. Specific examples of rinse solutions include the same developers as those exemplified in the "Development Step" section, as well as hydrocarbon solvents such as octane and heptane, and water. Here, the rinse solution may contain a surfactant. When selecting a rinse solution, it is preferable to select a rinse solution that is less likely to dissolve the resist film before the exposure step than the developer used in the development step and that is easily mixed with the developer.

[0086] <Etching Step> In the etching step, which can be optionally performed, the underlayer film and / or the substrate are etched using the above-mentioned resist pattern as a mask to form a pattern on the underlayer film and / or the substrate. In this case, the number of etchings is not particularly limited, and may be one or more times. Furthermore, the etching may be dry etching or wet etching, but dry etching is preferred. Dry etching can be performed using a known dry etching device. The etching gas used in dry etching can be appropriately selected depending on the elemental composition of the underlayer film and the substrate to be etched, etc. Examples of the etching gas include CHF 3 , C.F. 4 , C 2 F 6 , C 3 F 8 , SF 6 fluorine-based gases such as Cl 2 , BCl 3 Chlorine-based gases such as O 2 , O 3 , H 2 Oxygen-based gases such as O; 2 , N.H. 3 , CO, CO 2 , C.H. 4 , C 2 H 2 , C 2 H 4 , C 2 H6, C 3 H 4 , C 3 H 6 , C 3 H 8 , HF, HI, HBr, HCl, NO, BCl 3 reducing gases such as He, N 2 , and inert gases such as Ar. These gases may be used alone or in combination of two or more. For dry etching of an inorganic underlayer film, an oxygen-based gas is usually used. For dry etching of a substrate, a fluorine-based gas is usually used, and a mixture of a fluorine-based gas and an inert gas is preferably used.

[0087] Furthermore, if necessary, the underlayer film remaining on the substrate may be removed before or after etching the substrate. When the underlayer film is removed before etching the substrate, the underlayer film may be a patterned or unpatterned underlayer film.

[0088] Here, examples of methods for removing the underlayer film include the above-mentioned dry etching. In the case of an inorganic underlayer film, the underlayer film may be removed by contacting the underlayer film with a liquid such as a basic or acidic liquid, preferably a basic liquid. The basic liquid is not particularly limited, and examples thereof include alkaline hydrogen peroxide. The method for removing the underlayer film by wet stripping using alkaline hydrogen peroxide is not particularly limited as long as it allows the underlayer film and alkaline hydrogen peroxide to come into contact with each other for a certain period of time under heated conditions. Examples include a method of immersing the underlayer film in heated alkaline hydrogen peroxide, a method of spraying alkaline hydrogen peroxide onto the underlayer film in a heated environment, and a method of coating the underlayer film with heated alkaline hydrogen peroxide. After performing any of these methods, the substrate is washed with water and dried to obtain a substrate from which the underlayer film has been removed.

[0089] Below, an example of a method for forming a resist pattern using the positive resist composition of the present invention and a method for etching an underlayer film and a substrate using the formed resist pattern will be described. However, since the substrate used in the following example and the conditions in each step can be the same as the substrate and conditions in each step described above, explanations will be omitted below. It should be noted that the method for forming a resist pattern is not limited to the method shown in the following example.

[0090] An example of the resist pattern forming method is a resist pattern forming method using an electron beam or EUV, which includes the above-mentioned underlayer film forming step, resist film forming step, exposure step, developing step, and developer removing step.An example of the etching method is a method in which the resist pattern formed by the resist pattern forming method is used as a mask, and includes an etching step.

[0091] Specifically, in the underlayer film formation step, an inorganic material is applied to a substrate and baked to form an inorganic underlayer film. Next, in the resist film formation step, a positive resist composition of the present invention is applied to the inorganic underlayer film formed in the underlayer film formation step, and the composition is dried to form a resist film. Then, in the exposure step, the resist film formed in the resist film formation step is irradiated with EUV light to write a desired pattern. Furthermore, in the development step, the resist film exposed in the exposure step is brought into contact with a developer to develop the resist film, thereby forming a resist pattern on the underlayer film. Then, in the developer removal step, the resist film developed in the development step is brought into contact with a rinse solution to rinse the developed resist film. Then, in the etching step, the underlayer film is etched using the resist pattern as a mask to form a pattern in the underlayer film. Next, the substrate is etched using the patterned underlayer film as a mask to form a pattern on the substrate.

[0092] The present invention will be described in detail below based on examples, but the present invention is not limited to these examples. Furthermore, in a copolymer produced by copolymerizing multiple types of monomers, the proportion of a monomer unit formed by polymerizing a certain monomer in the copolymer usually coincides with the ratio (feed ratio) of that certain monomer to all monomers used in the polymerization of the copolymer, unless otherwise specified. In the examples and comparative examples, the proportion of the monomer unit in the copolymer, the calculated value of the lowest unoccupied molecular orbital (LUMO) of the monomer unit (I) in the copolymer, and the number-average molecular weight, weight-average molecular weight, and molecular weight distribution of the copolymer were measured or calculated using the following methods. In the examples and comparative examples, the exposure margin of the resist and the shape of the resist pattern were evaluated using the following methods. <Calculation of the lowest unoccupied molecular orbital (LUMO)> The lowest unoccupied molecular orbital (LUMO) value was calculated for the structure of the unit (monomer unit (I)) derived from monomer (a) using Psi4 (calculation level: b3lyp / 6-31G*). The lowest unoccupied molecular orbital (LUMO) is a calculated value based on the structure of a monomer unit having no polymerizable group. <Proportion of monomer units in copolymer> For the copolymers obtained in the preparation examples, 13The proportion of the monomer unit in the copolymer was calculated using the C-NMR method. Specifically, the copolymer obtained in the example was dissolved in chloroform-d, 99.8% (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) to a concentration of 10% by mass, and the resulting solution was analyzed using a nuclear magnetic resonance apparatus (manufactured by JEOL Ltd., 500 MHz). 13 C NMR spectra were measured, and the proportion of monomer units in the copolymer was calculated from the measurement results. <Number Average Molecular Weight, Weight Average Molecular Weight, and Molecular Weight Distribution> The number average molecular weight (Mn) and weight average molecular weight (Mw) of the copolymers obtained in the Examples, Comparative Examples, and Preparation Examples were measured using gel permeation chromatography, and the molecular weight distribution (Mw / Mn) was calculated. Specifically, a gel permeation chromatograph (Tosoh Corporation, HLC-8420) was used, and tetrahydrofuran was used as the developing solvent, to determine the number average molecular weight (Mn) and weight average molecular weight (Mw) of the copolymer in terms of standard polystyrene. The molecular weight distribution (Mw / Mn) was then calculated. <Exposure Margin> Resist patterns were formed using the positive resist compositions obtained in the Examples and Comparative Examples, and the exposure margin was evaluated. Specifically, a spin coater (Mikasa Corporation, MS-A150) was used to apply the positive resist composition to a thickness of 50 nm onto a 4-inch diameter silicon wafer. The applied positive resist composition was then heated on a hot plate at 170°C for 1 minute to form a resist film on the silicon wafer (resist film formation step). The resist film had a thickness of 50 nm. The resist film was then coated at 100 μC / cm using an electron beam lithography system (ELS-S50, manufactured by Elionix). 2 to 400 μC / cm 2 Within the range of 10 μC / cm 2The resist film was exposed to light at different exposure doses, and a pattern was written (exposure step). After the exposure step, the resist film was subjected to a development process using isopropyl alcohol (IPA) as a developer at a temperature of 23°C for 1 minute (development step). The developer was then removed by nitrogen blowing to form a resist pattern (developer removal step). The formed resist pattern was then observed for pattern separation and the presence or absence of pattern collapse. The lines (unexposed areas) and spaces (exposed areas) of the resist pattern were each set to 30 nm. The exposure margin was evaluated according to the following criteria. The results are shown in Table 2. A: The difference between the exposure dose at which pattern separation begins and the exposure dose at which pattern collapse occurs is 50 μC / cm 2 B: The difference between the exposure dose at which pattern separation begins and the exposure dose at which pattern collapse occurs is 10 μC / cm 2 More than 50μC / cm 2 C: The difference between the exposure dose at which pattern separation begins and the exposure dose at which pattern collapse occurs is less than 10 μC / cm 2 <Resist Pattern Shape> Resist patterns were formed using the positive resist compositions obtained in the Examples and Comparative Examples, and the resist pattern shapes were evaluated. Specifically, the shapes of patterns exposed at the median exposure dose within the range from pattern separation to pattern collapse when the exposure margin was evaluated above were observed using a scanning electron microscope. The shapes of the resist patterns were then evaluated according to the following criteria. The results are shown in Table 2. A: The sidewall shape of the resist pattern is smooth. B: The sidewall shape of the resist pattern is rough.

[0093] Example 1 Preparation of Copolymer A monomer composition A1 containing 3.46 g of α-chloroacrylate-4-t-butylcyclohexyl (ACATBCH) as the monomer (a), 1.64 g of α-methylstyrene (AMS) as the monomer (b), 0.0051 g of V-601 (dimethyl 2,2'-azobis(2-methylpropionate)) as a polymerization initiator, and 3.26 g of cyclopentanone as a solvent was placed in a glass container, the glass container was sealed and purged with nitrogen, and the mixture was stirred in a constant temperature bath at 78°C under a nitrogen atmosphere for 6 hours. The temperature was then returned to room temperature, and the glass container was opened to the atmosphere. To the resulting solution, 8.36 g of tetrahydrofuran (THF) was then added. The solution to which THF had been added was then dropped into 200 g of methanol as a solvent to precipitate a polymer. The solution containing the precipitated polymer was then filtered using a Kiriyama funnel to obtain a white coagulated product (copolymer A1). The ratio of the monomer units in the obtained copolymer A1 was 13 Calculation using C-NMR revealed that Copolymer A1 was a copolymer containing 51 mol % of α-chloroacrylate-4-t-butylcyclohexyl units and 49 mol % of α-methylstyrene units.

[0094] <Preparation of Positive Resist Composition> The copolymer A1 prepared as described above was dissolved in isoamyl acetate as a solvent to prepare a positive resist composition with a concentration of 2 mass%. Using the obtained positive resist composition, the exposure margin and resist pattern shape were evaluated. The results are shown in Table 2.

[0095] Example 2 Various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that in the preparation of the copolymer, instead of the monomer composition A1, a monomer composition A2 containing 3.47 g of α-chloroacrylate-4-t-butylcyclohexyl (ACATBCH) as the monomer (a), 1.64 g of α-methylstyrene (AMS) as the monomer (b), 0.0102 g of V-601 (dimethyl 2,2'-azobis(2-methylpropionate)) as the polymerization initiator, and 3.27 g of cyclopentanone as the solvent was used to prepare copolymer A2. The results are shown in Table 2. The obtained copolymer A2 was a copolymer containing 52 mol% of α-chloroacrylate-4-t-butylcyclohexyl units and 48 mol% of α-methylstyrene units.

[0096] Example 3 Various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that in the preparation of the copolymer, instead of the monomer composition A1, a monomer composition A3 containing 3.47 g of 4-t-butylcyclohexyl α-chloroacrylate (ACATBCH) as the monomer (a), 1.68 g of α-methylstyrene (AMS) as the monomer (b), 0.0254 g of V-601 (dimethyl 2,2'-azobis(2-methylpropionate)) as the polymerization initiator, and 3.60 g of cyclopentanone as the solvent was used to prepare copolymer A3. The results are shown in Table 2. The obtained copolymer A3 was a copolymer containing 50 mol % of 4-t-butylcyclohexyl α-chloroacrylate units and 50 mol % of α-methylstyrene units.

[0097] Example 4 Various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that in the preparation of the copolymer, instead of the monomer composition A1, a monomer composition A4 containing 2.38 g of α-chloroacrylate-t-butyl (ACATB) as the monomer (a), 1.68 g of α-methylstyrene (AMS) as the monomer (b), 0.0252 g of V-601 (dimethyl 2,2'-azobis(2-methylpropionate)) as the polymerization initiator, and 3.60 g of cyclopentanone as the solvent was used to prepare copolymer A4. The results are shown in Table 2. The obtained copolymer A4 was a copolymer containing 47 mol% of α-chloroacrylate-t-butyl units and 53 mol% of α-methylstyrene units.

[0098] Example 5 In the preparation of the copolymer, various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that in place of the monomer composition A1, a monomer composition A5 containing 9.77 g of 2,2,3,3-tetrafluoropropyl α-chloroacrylate (ACA4FP) as the monomer (a), 5.23 g of α-methylstyrene (AMS) as the monomer (b), 0.163 g of V-601 (dimethyl 2,2'-azobis(2-methylpropionate)) as the polymerization initiator, and 3.63 g of cyclopentanone as the solvent was used to prepare copolymer A5. The results are shown in Table 2. The obtained copolymer A5 was a copolymer containing 48 mol% 2,2,3,3-tetrafluoropropyl α-chloroacrylate units and 52 mol% α-methylstyrene units.

[0099] Example 6 Various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that in the preparation of the copolymer, instead of the monomer composition A1, a monomer composition A6 containing 6.54 g of 2,2,3,3-tetrafluoropropyl α-chloroacrylate (ACA4FP) as the monomer (a), 3.51 g of α-methylstyrene (AMS) as the monomer (b), 0.547 g of V-601 (dimethyl 2,2'-azobis(2-methylpropionate)) as the polymerization initiator, and 23.1 g of cyclopentanone as the solvent was used to prepare copolymer A6. The results are shown in Table 2. The obtained copolymer A6 was a copolymer containing 51 mol% 2,2,3,3-tetrafluoropropyl α-chloroacrylate units and 49 mol% α-methylstyrene units.

[0100] Example 7 Various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that in the preparation of the copolymer, instead of the monomer composition A1, a monomer composition A7 containing 5.14 g of 2,2,3,3-tetrafluoropropyl α-chloroacrylate (ACA4FP) as the monomer (a), 5.17 g of 3,4,5-trimethoxy-α-methylstyrene (3,4,5-triMOAMS) as the monomer (b), 0.00861 g of V-601 (dimethyl 2,2'-azobis(2-methylpropionate)) as the polymerization initiator, and 6.97 g of cyclopentanone as the solvent was used to prepare copolymer A7. The results are shown in Table 2. The obtained copolymer A7 was a copolymer containing 47 mol% 2,2,3,3-tetrafluoropropyl α-chloroacrylate units and 53 mol% 3,4,5-trimethoxy-α-methylstyrene units.

[0101] Example 8 In the preparation of the copolymer, various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that in place of the monomer composition A1, a monomer composition A8 containing 5.79 g of 2,2,3,3-tetrafluoropropyl α-chloroacrylate (ACA4FP) as the monomer (a), 4.21 g of 4-isopropyl-α-methylstyrene (4IPAMS) as the monomer (b), 0.0130 g of V-70 (2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile)) as the polymerization initiator, and 6.27 g of cyclopentanone as the solvent was used to prepare copolymer A8. The results are shown in Table 2. The obtained copolymer A8 was a copolymer containing 48 mol% of 2,2,3,3-tetrafluoropropyl α-chloroacrylate units and 52 mol% of 4-isopropyl-α-methylstyrene units.

[0102] Example 9 Various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that in the preparation of the copolymer, instead of the monomer composition A1, a monomer composition A9 containing 5.24 g of 2,2,3,3-tetrafluoropropyl α-chloroacrylate (ACA4FP) as the monomer (a), 4.76 g of 4-cyclohexyl-α-methylstyrene (4CHAMS) as the monomer (b), 0.0123 g of V-70 (2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile)) as the polymerization initiator, and 6.49 g of cyclopentanone as the solvent was used to prepare copolymer A9. The results are shown in Table 2. The obtained copolymer A9 was a copolymer containing 52 mol% of 2,2,3,3-tetrafluoropropyl α-chloroacrylate units and 48 mol% of 4-cyclohexyl-α-methylstyrene units.

[0103] Example 10 In the preparation of the copolymer, various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that in place of the monomer composition A1, a monomer composition A10 containing 1.04 g of 2,2,3,3-tetrafluoropropyl α-chloroacrylate (ACA4FP) as the monomer (a), 0.961 g of 3-trifluoromethyl-4-fluoro-α-methylstyrene (3TFM4FAMS) as the monomer (b), 0.00441 g of V-601 (dimethyl 2,2'-azobis(2-methylpropionate)) as the polymerization initiator, and 0.441 g of cyclopentanone as the solvent was used to prepare copolymer A10. The results are shown in Table 2. The obtained copolymer A10 was a copolymer containing 51 mol % of 2,2,3,3-tetrafluoropropyl α-chloroacrylate units and 49 mol % of 3-trifluoromethyl-4-fluoro-α-methylstyrene units.

[0104] Example 11 In the preparation of the copolymer, various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that in place of the monomer composition A1, a monomer composition A11 containing 1.09 g of 2,2,3,3-tetrafluoropropyl α-chloroacrylate (ACA4FP) as the monomer (a), 0.916 g of 3-trifluoromethyl-α-methylstyrene (3TFMAMS) as the monomer (b), 0.00449 g of V-601 (dimethyl 2,2'-azobis(2-methylpropionate)) as the polymerization initiator, and 0.386 g of cyclopentanone as the solvent was used to prepare copolymer A11. The results are shown in Table 2. The obtained copolymer A11 was a copolymer containing 48 mol% 2,2,3,3-tetrafluoropropyl α-chloroacrylate units and 52 mol% 3-trifluoromethyl-α-methylstyrene units.

[0105] Example 12 In the preparation of the copolymer, various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that in place of the monomer composition A1, copolymer A12 was prepared using a monomer composition A12 containing 1.18 g of 2,2,3,3-tetrafluoropropyl α-chloroacrylate (ACA4FP) as monomer (a), 0.823 g of 3,4-difluoro-α-methylstyrene (3,4-diFAMS) as monomer (b), 0.00491 g of V-601 (dimethyl 2,2'-azobis(2-methylpropionate)) as a polymerization initiator, and 0.450 g of cyclopentanone as a solvent. The results are shown in Table 2. The obtained copolymer A12 was a copolymer containing 49 mol% 2,2,3,3-tetrafluoropropyl α-chloroacrylate units and 51 mol% 3,4-difluoro-α-methylstyrene units.

[0106] Example 13 In the preparation of the copolymer, various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that in place of the monomer composition A1, copolymer A13 was prepared using a monomer composition A13 containing 1.24 g of 2,2,3,3-tetrafluoropropyl α-chloroacrylate (ACA4FP) as monomer (a), 0.764 g of 4-fluoro-α-methylstyrene (4FAMS) as monomer (b), 0.00519 g of V-601 (dimethyl 2,2'-azobis(2-methylpropionate)) as a polymerization initiator, and 0.482 g of cyclopentanone as a solvent. The results are shown in Table 2. The obtained copolymer A13 was a copolymer containing 51 mol% 2,2,3,3-tetrafluoropropyl α-chloroacrylate units and 49 mol% 4-fluoro-α-methylstyrene units.

[0107] Example 14 In the preparation of the copolymer, various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that in place of the monomer composition A1, a monomer composition A14 containing 0.929 g of 2,2,3,3-tetrafluoropropyl α-chloroacrylate (ACA4FP) as the monomer (a), 1.08 g of 3,5-bistrifluoromethyl-α-methylstyrene (BisTFMAMS) as the monomer (b), 0.00772 g of V-601 (dimethyl 2,2'-azobis(2-methylpropionate)) as the polymerization initiator, and 0.361 g of cyclopentanone as the solvent was used to prepare copolymer A14. The results are shown in Table 2. The obtained copolymer A14 was a copolymer containing 53 mol% 2,2,3,3-tetrafluoropropyl α-chloroacrylate units and 47 mol% 3,5-bistrifluoromethyl-α-methylstyrene units.

[0108] Example 15 In the preparation of the copolymer, various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that in place of the monomer composition A1, copolymer A15 was prepared using a monomer composition A15 containing 1.04 g of 2,2,3,3-tetrafluoropropyl α-chloroacrylate (ACA4FP) as monomer (a), 0.961 g of 3-trifluoromethyl-4-fluoro-α-methylstyrene (3TFM4FAMS) as monomer (b), 0.0174 g of V-601 (dimethyl 2,2'-azobis(2-methylpropionate)) as a polymerization initiator, and 1.26 g of cyclopentanone as a solvent. The results are shown in Table 2. The obtained copolymer A15 was a copolymer containing 52 mol% 2,2,3,3-tetrafluoropropyl α-chloroacrylate units and 48 mol% 3-trifluoromethyl-4-fluoro-α-methylstyrene units.

[0109] Example 16 In the preparation of the copolymer, various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that in place of the monomer composition A1, a monomer composition A16 containing 6.65 g of 2,2,3,4,4,4-hexafluorobutyl α-chloroacrylate (ACA6FB) as the monomer (a), 3.35 g of 4-fluoro-α-methylstyrene (4FAMS) as the monomer (b), 0.00911 g of V-601 (dimethyl 2,2'-azobis(2-methylpropionate)) as the polymerization initiator, and 2.49 g of cyclopentanone as the solvent was used to prepare copolymer A16. The results are shown in Table 2. The obtained copolymer A16 was a copolymer containing 51 mol% 2,2,3,4,4,4-hexafluorobutyl α-chloroacrylate units and 49 mol% 4-fluoro-α-methylstyrene units.

[0110] Comparative Example 1 In the preparation of the copolymer, various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that in place of the monomer composition A1, copolymer A17 was prepared using a monomer composition A17 containing 11.07 g of α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl (ACAFPh), 3.93 g of α-methylstyrene as monomer (b), 0.013 g of V-601 (dimethyl 2,2'-azobis(2-methylpropionate)) as a polymerization initiator, and 9.99 g of cyclopentanone as a solvent. The results are shown in Table 2. The obtained copolymer A17 was a copolymer containing 52 mol% of α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl units and 48 mol% of α-methylstyrene units.

[0111] Comparative Example 2 Various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that in the preparation of the copolymer, instead of the monomer composition A1, a monomer composition A18 containing 2.70 g of 2-adamantyl α-chloroacrylate (ACA2Ad), 5.30 g of α-methylstyrene (AMS) as the monomer (b), and 0.0019 g of V-601 (dimethyl 2,2'-azobis(2-methylpropionate)) as the polymerization initiator was used to prepare copolymer A18. The results are shown in Table 2. The resist formed using copolymer A18 could not be developed, and no resist pattern was obtained. Therefore, it was not possible to evaluate the exposure margin and shape pattern. The obtained copolymer A5 was a copolymer containing 51 mol % 2-adamantyl α-chloroacrylate units and 49 mol % α-methylstyrene units.

[0112] Comparative Example 3 Various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that in the preparation of the copolymer, instead of the monomer composition A1, a monomer composition A19 containing 7.58 g of methyl α-chloroacrylate (ACAM), 7.41 g of α-methylstyrene (AMS) as the monomer (b), and 0.0232 g of V-601 (dimethyl 2,2'-azobis(2-methylpropionate)) as the polymerization initiator was used to prepare copolymer A19. The results are shown in Table 2. The resist formed using copolymer A6 could not be developed, and no resist pattern was obtained. Therefore, it was not possible to evaluate the exposure margin and shape pattern. The obtained copolymer A19 was a copolymer containing 55 mol % of methyl α-chloroacrylate units and 45 mol % of α-methylstyrene units.

[0113] Comparative Example 4 Various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that in the preparation of the copolymer, instead of the monomer composition A1, a monomer composition A20 containing 4.63 g of 2,2,3,3,3-pentafluoropropyl α-chloroacrylate (ACAPFP), 5.37 g of α-methylstyrene (AMS) as the monomer (b), and 0.0119 g of V-601 (dimethyl 2,2'-azobis(2-methylpropionate)) as the polymerization initiator was used to prepare copolymer A20. The results are shown in Table 2. The resist formed using copolymer A20 could not be developed, and no resist pattern was obtained. The exposure margin and shape pattern could not be evaluated. The obtained copolymer A7 was a copolymer containing 49 mol % 2,2,3,3,3-pentafluoropropyl α-chloroacrylate units and 51 mol % α-methylstyrene units.

[0114] In Table 2, "EB" represents an electron beam, "ACATBCH" represents a-chloroacrylate-4-t-butylcyclohexyl unit, "ACATB" represents a-chloroacrylate-t-butyl unit, "ACA4FP" represents a-chloroacrylate-2,2,3,3-tetrafluoropropyl unit, "ACA6FB" represents a-chloroacrylate-2,2,3,4,4,4-hexafluorobutyl unit, "ACAFPh" represents a-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl unit, "ACA2Ad" represents a-chloroacrylate-2-adamantyl unit, "ACAM" represents a-chloroacrylate methyl unit, "ACAPFP" represents a-chloroacrylate-2,2,3,3,3-pentafluoropropyl unit, "AMS" represents a-methylstyrene unit, "3,4,5-triMOAMS" indicates a 3,4,5-trimethoxy-α-methylstyrene unit, "4IPAMS" indicates a 4-isopropyl-α-methylstyrene unit, "4CHAMS" indicates a 4-cyclohexyl-α-methylstyrene unit, "3TFM4FAMS" indicates a 3-trifluoromethyl-4-fluoro-α-methylstyrene unit, "3TFMAMS" indicates a 3-trifluoromethyl-α-methylstyrene unit, "3,4-diFAMS" indicates a 3,4-difluoro-α-methylstyrene unit, "4FAMS" indicates a 4-fluoro-α-methylstyrene unit, "BisTFAMS" indicates a 3,5-bistrifluoromethyl-α-methylstyrene unit, and "IPA" indicates isopropyl alcohol.

[0115] The results shown in Table 2 show that in Examples 1 to 16, which used copolymers containing predetermined monomer units with a calculated lowest unoccupied molecular orbital (LUMO) of −0.70 eV or more, the exposure margin was wide and resist patterns with good shapes could be formed.

[0116] According to the present invention, it is possible to provide a copolymer and a positive resist composition which are capable of forming a resist pattern which has a wide exposure margin and a good shape, and also to provide a method of forming a resist pattern which is capable of forming a resist pattern which has a wide exposure margin and a good shape.

Claims

1. A compound represented by the following formula (I): (In formula (I), R 1 is a halogen atom or an alkyl group substituted with a halogen atom, R 2 is an aliphatic group which may have a substituent (provided that when the aliphatic group is a bridged cyclic saturated hydrocarbon group, it has a substituent), R 3 and R 4 are hydrogen atoms, halogen atoms, unsubstituted alkyl groups or alkyl groups substituted with halogen atoms, and may be the same or different from each other. (In formula (II), R 5 , R 7 and R 8 are hydrogen atoms, halogen atoms, unsubstituted alkyl groups or alkyl groups substituted with halogen atoms, and may be the same or different from each other; R 6 is a halogen atom or an organic group, and p is an integer of 0 to 5, and the monomer unit (I) has a calculated lowest unoccupied molecular orbital (LUMO) of -0.70 eV or more.

2. The above R 2 The copolymer according to claim 1 , wherein is an aliphatic group having 1 to 20 carbon atoms which may have a substituent.

3. The above R 2 The copolymer according to claim 1 , wherein is an aliphatic group having an electron-donating group as a substituent.

4. A positive resist composition comprising the copolymer according to any one of claims 1 to 3 and a solvent.

5. A method for forming a resist pattern, comprising the steps of: forming a resist film using the positive resist composition according to claim 4; exposing the resist film; and developing the exposed resist film.

6. The method for forming a resist pattern according to claim 5, wherein the development is carried out using an alcohol-based solvent.

Citation Information

Patent Citations

  • Polymer and positive resist composition

    JP2020084007A

  • Photoresist compositions and methods of use

    WO2010091927A1

  • Compound, polymer, composition, composition for film formation, pattern forming method, method for forming insulating film, method for producing compound, iodine-containing vinyl polymer and method for producing acetylated derivative of same

    WO2021029395A1

  • Positive resist composition, resist film, pattern formation method, and method for manufacturing electronic device

    WO2021153466A1