Ceramic substrate, ceramic circuit board, semiconductor device, method for producing slurry, and method for applying release agent
By controlling the mold release agent distribution on ceramic substrates, the method addresses the challenge of reusing offcuts and defective materials, improving yield and performance, and reducing waste in ceramic substrate manufacturing.
Patent Information
- Application Number
- PCT/JP2024/011508
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional ceramic substrate manufacturing processes face challenges in reusing offcuts and defective materials due to difficulties in completely separating mold release agents, which leads to performance deterioration and hindered recycling, resulting in low yield and increased waste.
A method is developed to control the distribution of mold release agent components on ceramic substrates by measuring and adjusting the amount at specific points, allowing for the reuse of scraps in the slurry manufacturing process, thereby improving yield and reducing waste while maintaining performance.
The method enables the effective reuse of offcuts and defective materials, enhancing the yield of ceramic substrates with improved voltage resistance and mechanical properties, and reducing waste by optimizing the mold release agent distribution.
Smart Images

Figure JP2024011508_03102024_PF_FP_ABST
Abstract
Description
Ceramic substrate, ceramic circuit board, semiconductor device, slurry manufacturing method, and release agent application method
[0001] Embodiments of the present invention generally relate to a ceramic substrate, a ceramic circuit board, a semiconductor device, a method for producing a slurry, and a method for applying a release agent.
[0002] Ceramic substrates are produced by mixing raw materials such as ceramic powder and binder, forming them into a sheet, and then cutting the sheet into plate-shaped ceramic bodies, which are then sintered (these are also called green sheets). This manufacturing method aims to sinter many plate-shaped ceramic bodies at once, and involves stacking and sintering multiple plate-shaped ceramic bodies coated with a release agent. Coating the surfaces of the green sheets with a release agent prevents the resulting ceramic substrates (sintered plate-shaped ceramic bodies) from sticking together.
[0003] For example, Patent Document 1 describes a method for obtaining a plate-shaped ceramic sintered body with little waviness, i.e., a ceramic substrate, by controlling the composition of a release agent layer formed by applying boron nitride paste to the surface of a sheet-shaped ceramic compact and sintering the plate-shaped ceramic compact.
[0004] Meanwhile, in the conventional manufacturing process of ceramic substrates, scraps that are generated when cutting a sheet-shaped ceramic molded body to a desired size after coating it with a release agent, and sheet-shaped ceramic molded bodies and plate-shaped ceramic molded bodies that have defects such as holes, tears, or an excess or deficiency of the amount of release agent applied after coating the release agent, have been discarded as scrap materials.
[0005] It is desirable to reuse scraps, such as scraps and defective pieces of sheet-shaped ceramic compacts and plate-shaped ceramic compacts, as raw materials for ceramic substrates to improve yield and reduce waste. However, it is difficult to completely separate the release agent from the scraps generated after the release agent is applied, and when reused, the remaining release agent components cause a decrease in the performance of the ceramic substrate. This decrease in performance has also not been understood based on the distribution of the release agent components. For these reasons, the reuse of scraps generated after the release agent is applied has been hindered.
[0006] Patent No. 5673847
[0007] An object of the present invention is to provide a ceramic substrate, a ceramic circuit board, a semiconductor device, a method for producing a slurry, and a method for applying a release agent, which have a high yield even when a release agent component is contained.
[0008] The ceramic substrate of the embodiment is characterized in that, when the midpoint C1 of the line segment connecting the center P1 of the first surface and the center P2 of the second surface is defined as the midpoint C1, the amount of the release agent components measured at the center P1 of the first surface or the center P2 of the second surface is five times or more the amount of the release agent components measured at the midpoint C1.
[0009] 1 is a schematic cross-sectional view showing an example of a ceramic substrate according to an embodiment; 2 is a schematic view showing an example of a ceramic circuit board according to an embodiment; 3 is a schematic view showing an example of a semiconductor device; 4 is a view showing an example of a sheet-shaped ceramic compact; 5 is a view showing an example of a cutting step for cutting the sheet-shaped ceramic compact; 6 is a flowchart showing an example of a method for manufacturing a ceramic sintered body according to an embodiment; Embodiment
[0010] A ceramic substrate, a ceramic circuit board, a semiconductor device, a method for producing a slurry, and a method for applying a release agent according to embodiments will be described with reference to FIGS.
[0011] The ceramic substrate according to the embodiment is suitable for use in ceramic circuit boards and semiconductor devices to which conductor portions are bonded.
[0012] Ceramic substrates, ceramic circuit boards, and semiconductor devices according to embodiments will be described with reference to FIGS. 1 to 6. FIG. 1 shows a schematic cross-sectional view (a plane perpendicular to the front and back surfaces) illustrating an example of a ceramic substrate coated with a release agent. In the ceramic substrate according to the embodiment, reference symbol S1 refers to the first surface (front surface). Furthermore, the center of the first surface S1 is designated as center P1. Furthermore, reference symbol S2 refers to the second surface (back surface). Furthermore, the center of the second surface S2 is designated as center P2. FIG. 2 shows a ceramic circuit board in which a front copper plate and a back copper plate are disposed on both sides of the ceramic substrate via bonding layers. FIG. 3 shows a semiconductor device. FIG. 4 shows an example of a sheet-shaped ceramic molded body. Furthermore, FIG. 5 shows an example of a cutting process for cutting the sheet-shaped ceramic molded body.
[0013] A method for manufacturing a ceramic sintered body according to an embodiment is shown in Fig. 6. In Fig. 5, ST1 is a mixing step, ST2 is a molding step, ST3 is a release agent application step, ST4 is a cutting step, ST5 is a sintering step, and ST6 is a cleaning step.
[0014] In the drawings, reference numeral 1 denotes a ceramic circuit board (for example, a ceramic copper circuit board), reference numeral 2 denotes a ceramic substrate, reference numeral 3 denotes a copper plate (front copper plate) as a conductor, reference numeral 4 denotes a copper plate (back copper plate) as a conductor, reference numeral 5 denotes a bonding layer (active metal brazing material layer), reference numeral 6 denotes a bonding layer between the copper plate and a semiconductor element, reference numeral 7 denotes a semiconductor element, reference numeral 8 denotes a semiconductor device, reference numeral 11 denotes a sheet-shaped ceramic compact not containing an applied release agent (laying powder), reference numeral 12 denotes a plate-shaped ceramic compact not containing an applied release agent (laying powder), reference numeral 13 denotes scrap material not containing an applied release agent (laying powder), reference numeral 14 denotes a release agent, reference numeral 15 denotes a release agent layer, reference numeral 16 denotes a sheet-shaped ceramic compact including the sheet-shaped ceramic compact 11 and the release agent applied thereto, reference numeral 17 denotes a cutting jig, reference numeral 22 denotes a plate-shaped ceramic compact including the plate-shaped ceramic compact 12 and the release agent applied thereto, reference numeral 23 denotes the scrap material before cleaning, and reference numeral 24 denotes the scrap material after cleaning.
[0015] The ceramic circuit board 1 shown in FIG. 2 has a structure in which a circuit pattern is imparted to a copper plate 3 on one of the front and back surfaces, and a copper plate 4 on the other surface serves as a heat sink. For convenience, the copper plate 3 is referred to as the front copper plate, and the copper plate 4 is referred to as the back copper plate. In the ceramic circuit board 1 shown in FIG. 2, two front copper plates 3 are arranged on a ceramic substrate 2. The ceramic circuit board 1 according to the embodiment is not limited to this configuration, and may have a structure in which three or more front copper plates 3 are provided on the ceramic substrate 2, or a structure in which one front copper plate 3 is provided. Alternatively, the back copper plate 4 may have a circuit pattern imparted to it. Alternatively, the ceramic substrate 2 may have only a front copper plate 3 without a back copper plate 4.
[0016] 3 has the semiconductor element 7 provided in only one location, the semiconductor device 8 according to the embodiment is not limited to this configuration and may have the semiconductor element 7 provided in multiple locations. A plurality of semiconductor elements 7 may be provided on the front copper plate 3, which is one circuit portion.
[0017] 2 and 3 show the ceramic substrate 2 and the semiconductor device 8, respectively, with copper plates disposed on both sides thereof, but the ceramic substrate 2 and the semiconductor device 8 according to the embodiment are not limited to such a configuration. For example, an aluminum plate may be disposed as a heat sink instead of the back copper plate 4. Furthermore, while FIGS. 2 and 3 show the ceramic substrate 2 and the semiconductor device 8 having a bonding layer, the ceramic substrate 2 and the semiconductor device 8 according to the embodiment are not limited to such a configuration, and may or may not have a bonding layer 6 (they may be directly bonded).
[0018] The thickness of the ceramic substrate 2 according to the embodiment is preferably 0.1 mm or more and 3 mm or less. If the thickness of the ceramic substrate 2 is less than 0.1 mm, the strength may be insufficient. If the thickness is greater than 3 mm, the ceramic substrate 2 may become a thermal resistor, which may reduce the heat dissipation performance of the ceramic circuit board 1. More preferably, the thickness of the ceramic substrate 2 is 0.15 mm or more and 2 mm or less.
[0019] The shape of the front and back surfaces of the ceramic substrate 2 according to the embodiment is not particularly limited, and may be, for example, rectangular (including square) or substantially circular. When the shape of the front and back surfaces of the ceramic substrate 2 is rectangular, the centers P1 and P2 are the intersections of two diagonal lines. When the shape of the front and back surfaces of the ceramic substrate 2 is circular, the centers P1 and P2 are the centers of the circles. In either case, it is preferable that the major axis or diameter is 100 mm or more.
[0020] Specific examples of the material of the ceramic substrate 2 include a silicon nitride substrate, an aluminum nitride substrate, an aluminum oxide substrate, and an alusil substrate.
[0021] The silicon nitride substrate preferably has a three-point bending strength of 600 MPa or more. Increasing the strength of the substrate allows the substrate thickness to be reduced. Therefore, the three-point bending strength of the silicon nitride substrate is preferably 600 MPa or more, and even 700 MPa or more. The silicon nitride substrate can be thinned to a thickness of 0.40 mm or less, and even 0.30 mm or less. In addition, the silicon nitride substrate preferably has a thermal conductivity of 80 W / m·K or more. A silicon nitride substrate with a thermal conductivity of 80 W / m·K or more may be, for example, one with a thermal conductivity of 90 W / m·K or 130 W / m·K.
[0022] The three-point bending strength of an aluminum nitride substrate is generally about 300 to 450 MPa. On the other hand, the thermal conductivity of an aluminum nitride substrate is generally 160 W / m·K or more. Because the strength of an aluminum nitride substrate is low, the substrate thickness is preferably 0.60 mm or more.
[0023] Aluminum oxide substrates generally have a three-point bending strength of about 300 to 450 MPa, but are inexpensive. Arsil substrates generally have a high three-point bending strength of about 550 MPa, but have a thermal conductivity of about 30 to 50 W / m·K. An Arsil substrate is a substrate made of a sintered mixture of aluminum oxide and zirconium oxide.
[0024] The ceramic substrate 2 according to the embodiment is more preferably a nitride-based ceramic. Among nitride-based ceramics, the ceramic substrate 2 is preferably either a silicon nitride substrate or an aluminum nitride substrate from the viewpoint of thermal and mechanical properties. When a metal member and a ceramic substrate are joined using an active metal brazing filler metal, the nitride-based ceramic forms a reactant at the interface with the brazing filler metal that contributes to the bonding strength. For example, when an active metal brazing filler metal containing Ti is used for joining, the nitride-based ceramic reacts with the Ti in the brazing filler metal to form titanium nitride. These reactants strengthen the bond, thereby improving the bonding strength with metal members, particularly copper plates.
[0025] The ceramic substrate 2 according to the embodiment contains a release agent 14. The release agent 14 contained in the ceramic substrate 2 is the release agent applied to the sheet-shaped ceramic compact 11 in the release agent application step ST3 (shown in FIG. 6 ) before sintering, or is derived from scrap material 24, which is the raw material for the recycled slurry described below. The amount of the release agent 14 at the center P1 or P2 of the ceramic substrate 2 according to the embodiment is preferably at least five times the amount of the release agent 14 at the midpoint C1, which is the midpoint of the line segment connecting the centers P1 and P2. In addition to the above, it is more preferable that the ratio P1 / P2 of the amount of the release agent 14 at the center P1 to the amount of the release agent 14 at the center P2 be 0.5≦P1 / P2≦2. Furthermore, it is more preferable that the amount of the release agent 14 at the midpoint C1 be greater than 0 ppm by mass and less than or equal to 50 ppm by mass. By controlling the components of the release agent 14 of the ceramic substrate 2 as described above, the ceramic substrate 2 exhibits excellent voltage resistance and mechanical properties. In the manufacturing process of the ceramic substrate 2, the amount of the release agent 14 applied to the sheet-shaped ceramic compact 11, which will be described later, can be adjusted to control the amount of the release agent 14 at the center P1 or P2. In addition, in the manufacturing process of the slurry, which will be described later, the amount of the release agent 14 at the midpoint C1 can be controlled by adjusting the degree of cleaning of the scraps 23 generated after the release agent 14 is applied to the sheet-shaped ceramic compact 11 and the amount of the cleaned scraps 24 added to the slurry.
[0026] It is possible that the raw material composition of the ceramic substrate 2 contains, as an auxiliary agent, a component identical to the component of the release agent 14. However, if the amount of the component measured at the midpoint C1 is sufficiently small, for example, 300 mass ppm or less, the effect of the component as an auxiliary agent is not substantially manifested, and therefore the component is entirely regarded as a component of the release agent 14.
[0027] When the ceramic substrate 2 is used as a ceramic circuit substrate 1, it is preferable to provide at least one conductor on both or one of the front and back surfaces of the ceramic substrate 2. In the ceramic circuit substrate 1 according to the embodiment, the conductor may be provided directly on the ceramic substrate 2, or may be provided via a brazing material layer 5. In the ceramic circuit substrate 1 according to the embodiment, the conductor may be provided after being bonded by being given a circuit shape in advance by cutting or punching, or may be provided by being bonded by etching. In addition, when conductors are provided on the front and back surfaces of the ceramic substrate 2, the conductor provided on the front surface and the conductor provided on the back surface may have the same thickness or different thicknesses.
[0028] In the circuit board 1 according to the embodiment, the conductor portion is preferably one or more of copper, copper alloy, aluminum, or aluminum alloy. More preferably, the conductor portion is copper or a copper alloy. Copper or a copper alloy has superior thermal conductivity compared to aluminum or an aluminum alloy. Generally, copper has a high thermal conductivity of approximately 400 W / m·K, which can improve the heat dissipation of the ceramic circuit board 1. More preferably, the conductor portion made of copper or a copper alloy is oxygen-free copper or a copper layer having a graphite layer present therein. Aluminum or an aluminum alloy is cheaper than copper, so is preferred when cost is a priority.
[0029] Furthermore, when the conductor is made of copper or a copper alloy, the thickness of the conductor may be 0.3 mm or more, or even 0.6 mm or more. A conductor made of copper or a copper alloy and having a thickness of 0.6 mm or more may be, for example, a 1 mm copper plate or a 2 mm copper plate. By making the conductor thicker, the heat dissipation properties of the bonded body can be improved.
[0030] From the above, the ceramic circuit board 1 according to the embodiment is preferably a ceramic copper circuit board. Here, the ceramic copper circuit board refers to a circuit board having a conductor portion made of copper or a copper alloy as a circuit.
[0031] The ceramic circuit board 1 according to the embodiment may have a heat dissipation member as a conductor. The heat dissipation member may have a shape that protrudes from the ceramic substrate (for example, a heat dissipation plate integrated with a lead frame), or may have a groove shape. Furthermore, the heat dissipation member may have a recess on its surface.
[0032] When the ceramic circuit board 1 according to the embodiment includes a brazing filler metal, the type of brazing filler metal constituting the brazing filler metal layer 5 may vary depending on the type of ceramic and conductor constituting the ceramic circuit board 1. However, for example, when the ceramic is a nitride-based ceramic and the conductor is copper or a copper alloy, the brazing filler metal preferably contains one or more of silver, copper, and an active metal. Preferably, the active metal is at least one metal selected from Ti, Zr, Nb, and Hf. The brazing filler metal may be, for example, an Al-Ti alloy, a Cu-Mg alloy, a Cu-Ti alloy, or an Ag-Ti alloy, which are composed of only two metal components (excluding unavoidable impurities). Alternatively, the brazing filler metal may be an Ag-Cu-Ti alloy, a Cu-Sn (or In or Mn)-Ti alloy, or an Ag-Cu-Sn (or In or Mn)-Ti alloy, which are composed of three or more metal components (excluding unavoidable impurities). The term "Sn (or In or Mn)" used herein refers to at least one metal species (or two or three metal species) selected from the three types of Sn, In, and Mn.
[0033] Among the brazing filler metal compositions described above, those containing active metals are preferred. Even more preferred are those containing at least one of Ag (silver) and Cu (copper) in a total content of 50 wt% to 99 wt%. Even more preferred are those containing Sn (or In or Mn) in a proportion of 0.5 wt% to 35 wt%. Even more preferred are those containing active metals in a total content of 0.5 wt% to 25 wt%.
[0034] The thickness of the brazing filler metal layer 5 is preferably 5 μm or more and 45 μm or less. More preferably, the thickness of the brazing filler metal layer 5 is 10 μm or more and 25 μm or less. If the thickness of the brazing filler metal layer 5 is less than 5 μm, there is a risk that sufficient strength will not be maintained. On the other hand, if the brazing filler metal layer 5 is thicker than 45 μm, there is a risk that problems such as cracks at the bonding interface and warping of the ceramic circuit board 1 will occur due to the difference in thermal expansion coefficient between the ceramic substrate 2 and the bonding layer 6.
[0035] The brazing filler metal layer 5 is formed by joining the ceramic substrate 2 and the conductor portion by brazing. When brazing the ceramic substrate 2 and the conductor portion, for example, a brazing filler metal paste or a brazing filler metal foil may be used. When using a brazing filler metal paste, the brazing filler metal paste may be applied multiple times, or multiple times with different compositions.
[0036] In the semiconductor device 8 according to the embodiment, a semiconductor element 7 is provided on a conductor portion of a circuit board 1 according to the embodiment, for example, via a bonding layer 6. The bonding layer 6 is formed by bonding the conductor portion and the semiconductor element 7 with, for example, a solder material or a conductive adhesive. When bonding the conductor portion and the semiconductor element 7 with a conductive adhesive, for example, a silver paste containing silver as a main component or a copper paste containing copper as a main component can be used as the conductive adhesive. Silver paste is preferred because it is resistant to oxidation. Copper paste is cheaper than silver paste, so it is preferred when cost is a priority.
[0037] The semiconductor element 7 may be, for example, a silicon carbide (SiC) power semiconductor or a gallium nitride (GaN) power semiconductor.
[0038] The method for producing the slurry according to the embodiment will be described. The method for producing the slurry according to the embodiment includes a cleaning step ST6 (shown in FIG. 6 ) for cleaning scraps 23 obtained by cutting the sheet-shaped ceramic compact 16 coated with the release agent 14, and a mixing step ST1 for adding and mixing the scraps 24 from which part of the release agent 14 has been separated in the cleaning step ST6 with a new slurry containing ceramic powder, a binder, a sintering aid, and the like to obtain a recycled slurry.
[0039] First, scraps 23 are prepared by cutting the sheet-shaped ceramic compact 16 coated with the release agent 14. The scraps 23 are produced through steps ST1 to ST4. Note that the scraps 23 prepared here may be scraps 23 produced without adding recycled raw materials such as the scraps 24 in the mixing step ST1, i.e., scraps produced only from new slurry.
[0040] In the mixing step ST1 (shown in FIG. 6 ), ceramic powder, binder, sintering aid, etc. are mixed to obtain a slurry. Examples of ceramic powder include powders primarily composed of silicon nitride, aluminum nitride, aluminum oxide, zirconium oxide, and silicon carbide. The type of ceramic powder is selected depending on the primary component of the desired ceramic substrate (plate-shaped ceramic sintered body). Here, the primary component of the sheet-shaped ceramic compact 11, the plate-shaped ceramic compact 22, and the plate-shaped ceramic sintered body produced by sintering them refers to the component with the largest mass ratio among the components constituting the sheet-shaped ceramic compact 11, the plate-shaped ceramic compact 22, and the plate-shaped ceramic sintered body. The sheet-shaped ceramic compact 11 primarily composed of silicon nitride becomes a silicon nitride sintered body after sintering. Similarly, the sheet-shaped ceramic compact 11 primarily composed of aluminum oxide becomes an aluminum oxide sintered body after sintering.
[0041] In the forming step ST2 (shown in FIG. 6 ), a sheet-shaped ceramic green body 11 is formed from the slurry by a doctor blade method, die molding, cold isostatic pressing (CIP), injection molding, or the like. The doctor blade method is preferred when producing a ceramic substrate. The doctor blade method can produce a long sheet-shaped ceramic green body 11. This can improve the mass productivity of ceramic substrates (plate-shaped ceramic sintered bodies). Hereinafter, an example of obtaining a sheet-shaped ceramic green body 11 by the doctor blade method will be described.
[0042] In the forming step ST2 (shown in FIG. 6 ), the sheet-shaped ceramic green body 11 is subjected to a degreasing treatment as needed. The degreasing treatment is also included in the sheet-shaped ceramic green body 11. The degreasing treatment may be performed on the sheet-shaped ceramic green body 11 in the forming step ST2 before the application of the release agent 14, on the sheet-shaped ceramic green body 16 after the application of the release agent 14, or on the plate-shaped ceramic green body 22 after cutting. The sheet-shaped ceramic green body 16 also includes a degreasing treatment on the sheet-shaped ceramic green body 16, and the plate-shaped ceramic green body 22 also includes a degreasing treatment on the plate-shaped ceramic green body 22.
[0043] Subsequently, in a release agent application step ST3 (shown in FIG. 6), a release agent 14 is applied to the sheet-shaped ceramic compact 11 to provide a release agent layer 15. Methods for applying the release agent 14 to the sheet-shaped ceramic compact 11 include, for example, using a spray, passing the compact through a solution containing the laying powder 4, using a brush, using static electricity, gravure printing, and immersing the compact in a solution containing the laying powder 4. Subsequently, in a cutting step ST4 (shown in FIG. 6), the sheet-shaped ceramic compact 16 to which the release agent 14 is attached is cut to a desired size.
[0044] In the manufacturing process of the ceramic substrate 2, the sheet-shaped ceramic green body 16 is generally cut into the desired size using, for example, a cutting jig 17 (shown in FIG. 5 ). Here, such a green body before application of the release agent and cutting is referred to as the sheet-shaped ceramic green body 11 (shown in FIG. 4 ), the green body before cutting in which the sheet-shaped ceramic green body 11 is coated with the release agent 14 is referred to as the sheet-shaped ceramic green body 16 (shown in FIG. 4 ), and each green body obtained by cutting the sheet-shaped ceramic green body 16 is referred to as the plate-shaped ceramic green body 22 (shown in FIG. 5 ). The sheet-shaped ceramic green body 16 is formed by applying the release agent 14 to the sheet-shaped ceramic green body 11 and forming a release agent layer 15 on the sheet-shaped ceramic green body 11. The plate-shaped ceramic green body 22 is formed by forming the release agent layer 15 on the plate-shaped ceramic green body 12.
[0045] Here, the scrap 23 refers to offcuts generated when cutting the sheet-shaped ceramic compact 16 to the desired size, etc. Additionally, the scrap 23 refers to waste products that have defects such as holes, tears, excessive or insufficient thickness, or excessive or insufficient application of release agent. Additionally, the scrap 23 refers to the sheet-shaped ceramic compact 16 or the plate-shaped ceramic compact 22 that are reused as other slurry raw materials, or components of the sheet-shaped ceramic compact 16 or the plate-shaped ceramic compact 22 obtained in the form of chips, etc. Hereinafter, the scrap of the sheet-shaped ceramic compact 16 or the plate-shaped ceramic compact 22 to which the release agent 14 has been applied may also be referred to simply as "scrap."
[0046] In this embodiment, the release agent 14 is, for example, one or more selected from boron nitride, zirconium oxide, aluminum oxide, and aluminum nitride. The release agent 14 serves to prevent the plate-shaped ceramic compacts 22 from adhering to each other when stacking and sintering the compacts. The release agent 14 preferably has an average particle size of 20 μm or less. If the average particle size exceeds 20 μm, the amount of application may become uneven, which may adversely affect the surface properties of the sintered compact. Preferably, the average particle size of the release agent 14 is 10 μm or less, more preferably 6 μm or less. There is no particular lower limit to the average particle size of the release agent 14, but a value of 2 μm or more is preferred. If the average particle size is less than 2 μm, handling may be impaired.
[0047] Next, a washing step is carried out in which the release agent 14 is separated from the scraps 23 by washing, and the scraps 24 from which a part of the release agent 14 has been separated are collected.
[0048] It is preferable to make the scraps 23 uniform in size before cleaning them. Therefore, if the scraps 23 are different in size, it is preferable to cut them to approximately the same size. Here, "approximately the same" means that the average value of the front and back surface areas of the scraps 23 is at least one-third of the maximum value. The closer the front and back surface areas of the scraps 23 are to each other, the less likely unevenness occurs in the removal of the release agent 14. Furthermore, when the scraps 23 are reused as a slurry raw material, the dispersion of the components of the release agent 14 in the slurry is easily homogenized, and scraps 23 with an adhesion amount of the components of the release agent 14 of approximately 50 ppm by mass can be reused without any problems.
[0049] The area of the front and back surfaces of the scrap 23 is 2 cm 2 It is preferable that the area of the front and back surfaces of the scrap 23 is 2 cm or more. 2 If the scrap 23 has a fine shape of less than 100 cm, the amount of cleaning liquid adhering to the scrap 23 increases, and it may take a long time to dry. There is no particular upper limit to the area of the front and back surfaces of the scrap 23, but in order to improve the efficiency of cleaning, it is preferable to use a size of 100 cm. 2 If the scrap 23 is not in a sheet or plate shape, any other appropriate criteria such as the surface area or apparent surface area may be used instead of the area of the front and back surfaces.
[0050] The cleaning of the scraps 23 in the cleaning step ST6 (shown in FIG. 6) is preferably performed by ultrasonic cleaning. Using ultrasonic cleaning improves the cleaning effect and reduces the cleaning time and number of cleanings. The temperature of the cleaning liquid used to clean the scraps 23 is preferably 5°C or higher and 60°C or lower. If the temperature of the cleaning liquid is 5°C or higher, the efficiency of drying after cleaning can be improved. On the other hand, if the temperature of the cleaning liquid is 60°C or lower, binder denaturation is less likely to occur. It is more preferable that the temperature of the cleaning liquid is 15°C or higher and 40°C or lower.
[0051] The cleaning liquid used to clean the scrap material 23 is not particularly limited, but is preferably a solution containing water as a solvent and a water-soluble auxiliary agent added thereto. Examples of the water-soluble auxiliary agent include organic compounds having hydrophilic groups such as carboxyl groups, alcohol groups, amino groups, thiol groups, sulfo groups, phosphate groups, and ketone groups, or salts thereof. Cleaning of the scrap material 23 may be performed using multiple types of cleaning liquids.
[0052] A surfactant may be added to the cleaning solution used to clean the scraps 23 in order to prevent redeposition of the components of the release agent 14. The surfactant to be added may be either a nonionic or ionic surfactant. When an ionic surfactant is added, any of anionic surfactants, cationic surfactants, and amphoteric surfactants may be used, but it is preferable to use an amphoteric surfactant.
[0053] If anionic surfactants and cationic surfactants remain in the scrap material 24 after washing, there is a risk that they may affect the sinterability of the plate-shaped ceramic molding 22 obtained by molding when the washed scrap material 24 described below is used as a slurry raw material.
[0054] Examples of anionic surfactants include carboxylic acid surfactants, sulfonic acid surfactants, sulfate ester surfactants, and phosphate ester surfactants. Examples of cationic surfactants include alkylamine salts and quaternary ammonium salts. Examples of amphoteric surfactants include carboxybetaine surfactants, 2-alkylimidazoline derivatives, glycine surfactants, and amine oxide surfactants. It is also preferable that the surfactant used be a nonionic surfactant. Examples of nonionic surfactants include ester, ether, ester ether, and alkanolamide surfactants. When using a nonionic surfactant, a polyhydric alcohol-based surfactant or a polyoxyethylene-based surfactant may be used. When using a nonionic surfactant, ions do not remain in the scrap 24 after cleaning. This prevents a decrease in sinterability during reuse.
[0055] From the above, it is particularly preferable that the cleaning solution used to clean the scraps 23 is one in which water is used as a solvent and a water-soluble auxiliary is added, and that the water-soluble auxiliary is primarily composed of an amphoteric surfactant or a nonionic surfactant that is composed of three or more atoms selected from carbon (C), hydrogen (H), oxygen (O), and nitrogen (N) and does not contain any other atoms. When the cleaned scraps 24 are used as a slurry raw material, even if these remain in the cleaned scraps 24 and are mixed into the slurry, they are unlikely to affect the sinterability.
[0056] Furthermore, when this surfactant has a linear chain portion, it is preferable that the number of carbon atoms in the linear chain portion is 25 or less. If the number of carbon atoms in the linear chain portion is small, it is possible to prevent the binder contained in the scrap 23 from dissolving in the cleaning liquid. On the other hand, if the number of carbon atoms is too large, it may not dissolve sufficiently in the cleaning liquid, making it difficult to separate the components of the release agent 14 from the scrap 23. By controlling the number of carbon atoms, it becomes easier to separate the components of the release agent 14 from the scrap 23.
[0057] The cleaning liquid may also be an inorganic compound solution. The inorganic compound solution may be a solution containing a gas such as carbon dioxide, nitrogen, oxygen, or argon as a solute. When a gas is used, bubbles of the gas are expected to remove components of the release agent 14 adhering to the scrap material 23 when they burst in water. When the gas component is used, it is more preferable to control the temperature of the cleaning liquid to 5°C or higher. When the temperature of the cleaning liquid is 5°C or higher, the solubility of the gas component in water is sufficiently improved, thereby reducing variation in the cleaning effect.
[0058] The number of times the scraps 23 are washed and the amount of auxiliary agent added to the cleaning solution may be freely selected depending on the purpose. Therefore, there are no particular limitations on the number of times the scraps 23 are washed or the amount of auxiliary agent added. After washing, the scraps 24 may be removed from the cleaning solution all at once using a sieve or the like, or they may be removed one by one. When using a sieve-like tool for removal, it is preferable to use one with openings large enough to allow the cleaning solution, release agent 14, etc. to pass through.
[0059] The solution containing the release agent 14 produced by washing the scraps 23 in the washing step ST6 (shown in FIG. 6 ) can be separated into the release agent 14 component and the solution component by, for example, leaving the solution to settle, or by filtration or centrifugation, and the solution component can be reused as a washing liquid. The release agent 14 component separated from the scraps 23 can be reused as the release agent 14 to be applied to a new sheet-shaped ceramic compact 11. Furthermore, the contents of the release agent 14 component and other components can be adjusted to prepare a solution for application of the release agent 14.
[0060] Next, a mixing step ST1 (shown in FIG. 6 ) is performed in which the washed scraps 24 are added to and mixed with new slurry to obtain a recycled slurry. When adding the washed scraps 24 to the new slurry, it is preferable that the amount of the washed scraps 24 added is 25% by mass or less, assuming that the powdered raw material of the new slurry is 100% by mass. A more preferable amount is 5% by mass or more and 20% by mass or less. If the amount of the washed scraps 24 added is less than 5% by mass relative to 100% by mass of the powdered raw material of the slurry, the benefits of recycling may not be fully obtained. On the other hand, if the amount exceeds 25% by mass, more thorough washing may be required, such as by increasing the number of times, which may increase the cost of washing.
[0061] When adding the scraps 24 to the new slurry, it is preferable to wet mix them using a bead mill or a ball mill. During the wet mixing, it is preferable to add a predetermined amount of binder component that is larger than usual. Furthermore, as described above, after adding the predetermined amount of binder component, it is preferable to add a solvent until the predetermined viscosity is reached.
[0062] The component ratio of the washed scraps 24 differs from the desired component ratio for the slurry due to volatilization during the manufacturing process. As described above, adjusting the binder and solvent components and adding the washed scraps 24 can compensate for the missing components and produce a regenerated slurry with the desired component ratio. Furthermore, during the mixing process, any cracks or thickness defects that occurred during the drying process before application of the release agent 14 may also be added. As described above, by further mixing the scraps before application of the release agent 14 components, the number of ceramic sintered bodies that can be produced per raw material powder can be increased, further improving the yield per raw material amount. In this case, the total amount of the powder raw material in the slurry is preferably 100% by mass, and the total amount of the washed scraps 24 and the sheet-shaped ceramic compacts 11 before application of the release agent 14 is preferably 25% by mass or less. Preferably, this total is 5% by mass or more and 20% by mass or less.
[0063] Furthermore, when a slurry of a ceramic sintered body using alumina as a raw material is produced by the method of the embodiment, if an alumina sintered body is used as a media for a bead mill or a ball mill, the amount of alumina added to the raw material may be controlled in consideration of alumina that is mixed in due to wear of the media.
[0064] After steps ST1 to ST4 using new slurry and steps ST1 to ST4 using recycled slurry (based on scrap material 24), the plate-shaped ceramic compact 22 is sintered in a sintering step ST5 (shown in FIG. 6) to produce a plate-shaped ceramic sintered body, i.e., a ceramic substrate. In the sintering step ST5, sintering is performed by heat treatment under normal pressure or pressure, typically at 1600 to 2000°C. Alternatively, the sintering step ST5 may be configured to perform a two-stage heat treatment using different temperature ranges for the heat treatment.
[0065] In addition, recycled release agent 14 may be applied in the release agent application step ST3 (shown in FIG. 6 ). In this case, the release agent component application method includes, for example, a washing step ST6 in which the scrap material 23 is washed to obtain ceramic sintered body pieces from which a portion of the release agent 14 has been separated; an adjustment step in which the content of the separated release agent 14 is adjusted to prepare a solution containing the release agent 14; a dispersion step in which the concentration of the release agent 14 contained in the solution prepared in the adjustment step is uniformly dispersed; and an application step in which the solution obtained through the dispersion step is applied to the sheet-shaped ceramic compact 11. The release agent application step ST3 includes, for example, the application step, in which the solution obtained through the dispersion step is applied to the sheet-shaped ceramic compact 11. In the application step, it is preferable to apply the release agent 14 to the sheet-shaped ceramic compact 11 using a spray method. The spray method allows for a stable spray amount of the release agent 14. Furthermore, by providing multiple spray nozzles, the release agent 14 can be applied over a wide area. In the case of the spray method, the long sheet-shaped ceramic compact 11 can be placed and transferred while being coated with the release agent 14. In the case of the spray method, a solution containing the release agent 14 may be sprayed.
[0066] (Example) A ceramic sheet 11 containing silicon nitride and aluminum nitride as its main components was prepared, and boron nitride was applied as a mold release agent 14. After that, the ceramic sheet 16 coated with the mold release agent 14 was cut into a size of 15 cm2. 2 The ceramic green body was cut into smaller pieces to produce plate-shaped ceramic green bodies (hereinafter referred to as "ceramic green body pieces") as simulants of the scrap material 23. Then, in the cleaning step ST6 (shown in FIG. 6), the ceramic green body pieces were cleaned using a first cleaning liquid (cleaning liquid 1), a second cleaning liquid (cleaning liquid 2), and a third cleaning liquid (cleaning liquid 3). Table 1 shows the materials of the sheet-shaped ceramic green bodies 11 constituting the ceramic green body pieces according to Examples 1 to 5 and Comparative Examples 1 and 2, as well as the causes of defects in the ceramic green body pieces and cleaning methods.
[0067] The composition formulas entered in the "Sheet" column of Table 1 indicate the type of material of the sheet-like ceramic compact 11 constituting the ceramic compact pieces according to Examples 1 to 5 and Comparative Examples 1 and 2, as the type of ceramic substrate after sintering. 3 N 4 is a ceramic substrate containing silicon nitride as the main component (50 mass % or more), and similarly, AlN is a ceramic substrate containing aluminum nitride as the main component (50 mass % or more).
[0068] The ceramic molded body pieces marked "small" in the column for the cause of defect in Table 1 are normal in the amount of release agent 14 applied and in the presence or absence of shape defects, but are smaller than the required size. The ceramic molded body pieces marked "crack" in the column for the cause of defect in Table 1 are normal in the amount of release agent 14 applied and in the size, but are defective in the shape (crack, break, or hole). The ceramic molded body pieces marked "unevenness" in the column for the cause of defect in Table 1 are normal in the size and the presence or absence of shape defects, but are defective in the amount applied, such as in the case where the unevenness in the amount of release agent 14 applied is too large or the amount applied on one side is too small.
[0069] In the first cleaning step and the second cleaning step in Table 1, the cleaning described as "Clean 1" is the rough cleaning, the cleaning described as "Clean 2" is the main cleaning, and the cleaning described as "Clean 3" is the finish cleaning. Different types of cleaning solutions were used for the rough cleaning, the main cleaning, and the finish cleaning.
[0070] In Examples 1 and 3, ultrasonic cleaning was performed for all cleaning steps, whereas in Examples 2, 4, and 5 and Comparative Examples 1 and 2, ultrasonic cleaning was not performed.
[0071] [Table 1]
[0072] Next, the amount of release agent 14 adhering to the surface of the ceramic molded body piece was measured before and after the cleaning step. Table 2 shows the results, with ceramic molded body pieces whose surface adhesion amount (ratio) of release agent 14 after cleaning was more than 0 ppm by mass and not more than 25 ppm by mass being labeled "A," ceramic molded body pieces whose surface adhesion amount (ratio) of release agent 14 after cleaning was more than 25 ppm by mass and not more than 50 ppm by mass being labeled "B," and ceramic molded body pieces whose surface adhesion amount (ratio) was more than 50 ppm by mass being labeled "D."
[0073] Next, the surface adhesion amount of the release agent 14 before cleaning was compared with the surface adhesion amount of the release agent 14 after cleaning. The surface adhesion amount of the release agent 14 before cleaning relative to the surface adhesion amount of the release agent 14 after cleaning (before removal / after removal) is shown in Table 2. This ratio is a value indicating the cleaning efficiency. The cleaning efficiency of the ceramic molded body pieces according to Examples 1 to 5 was in a preferable range (40% or more).
[0074] [Table 2]
[0075] Next, in step ST1, the washed ceramic molded pieces were mixed with new slurry raw material powder of the ceramic substrate to prepare a regenerated slurry. The mass ratio (%) of the washed ceramic molded pieces to the raw material powder in Examples 1 to 5 and Comparative Examples 1 and 2 is shown in Table 3.
[0076] The obtained slurry was formed into a sheet-shaped ceramic compact 11, and a release agent 14 was applied to the sheet-shaped ceramic compact 11. The ceramic compact piece coated with the release agent 14 was then subjected to degreasing and sintering to obtain a ceramic substrate. Boron nitride was used as the release agent 14. In the release agent application step ST3, the release agent 14 was a mixture of boron nitride powder and water, which was applied to the sheet-shaped ceramic compact 11 by spraying.
[0077] The ceramic substrates obtained by sintering were subjected to pressure resistance tests and bending strength tests. For comparison, a comparative ceramic substrate (hereinafter referred to as a "standard ceramic substrate") was prepared under the same conditions using a new slurry instead of the recycled slurry, and similar tests were conducted. In the pressure resistance test, a constant voltage was applied to the ceramic substrates based on the recycled slurry from the ceramic compact pieces according to Examples 1 to 5 and Comparative Examples 1 and 2, and the standard ceramic substrates based on the new slurry, and the leakage current values were compared. The results of the pressure resistance tests for the ceramic substrates according to Examples 1 to 5 and Comparative Examples 1 and 2 are shown in Table 3. Those with a current increase of 0% or more but less than 0.5% are labeled "A," those with a current increase of 0.5% or more but less than 0.75% are labeled "B," those with a current increase of 0.75% or more but less than 1.0% are labeled "C," and those with a ground fault are labeled "D."
[0078] In the bending strength test, the three-point bending strength of the ceramic substrates based on the recycled slurries from the ceramic molded body pieces according to Examples 1 to 5 and Comparative Examples 1 and 2, and the standard ceramic substrates based on the new slurries, was measured in accordance with JIS R 1601. Regarding the bending strength test of the ceramic substrates according to Examples 1 to 5 and Comparative Examples 1 and 2, those that were 99% or more of the standard ceramic substrate were rated as "A", those that were 96% or more but less than 99% were rated as "B", those that were 94% to less than 96% were rated as "C", and those that were less than 94% were rated as "D". These are shown in Table 3.
[0079] [Table 3]
[0080] Furthermore, the amounts of components of the release agent 14 at the midpoint C1 were controlled in the cleaning process and the slurry production process for the ceramic substrates of Examples 1 to 5. The amounts of components of the release agent 14 at the center P1 of the first surface S1, the center P2 of the second surface S2, and the midpoint C1 of the ceramic substrates of Examples 1 to 5 and Comparative Examples 1 and 2 were measured using an ICP optical emission spectrometer.
[0081] For each of the ceramic substrates of Examples 1 to 5 and Comparative Examples 1 and 2, the ratio (mP1) / (mC1) of the component amount of the release agent 14 measured at the center P1 (or center P2) (referred to as mP1) to the component amount of the release agent 14 measured at the midpoint C1 (referred to as mC1) was calculated. The calculation results are shown in Table 4. The ratio (mP1) / (mC1) for the ceramic substrates of Examples 1 to 5 was 5 or more. Furthermore, the component amount mC1 of the release agent 14 measured at the midpoint C1 was less than 30 ppm by mass in Examples 1 and 3, 30 ppm by mass or more and less than 40 ppm by mass in Example 2, and 40 ppm by mass or more and 50 ppm by mass or less in Examples 4 and 5. On the other hand, in both Comparative Examples 1 and 2, the component amount exceeded 50 ppm by mass, and the component amount of the release agent 14 was greater in Comparative Example 1 than in Comparative Example 2.
[0082] [Table 4]
[0083] Furthermore, the ratio P1 / P2 of the component amount of the release agent 14 at the center P1 of the first surface S1 to the component amount of the release agent 14 at the center P2 of the second surface S2 opposite the first surface S1 was 0.5≦P1 / P2≦2 in all of Examples 1 to 5. Furthermore, the component amount of the release agent 14 at the midpoint C1 was greater than 0 ppm by mass and not more than 50 ppm by mass in all of Examples 1 to 5.
[0084] Therefore, in Table 3, when the midpoint C1 is defined as the midpoint of the line segment connecting the center P1 of the first surface S1 and the center P2 of the second surface S2 of the ceramic substrate, the ceramic substrate having excellent voltage resistance and mechanical strength (for example, bending strength) has the components of the release agent 14 measured at the center P1 (or the center P2) five times or more the components of the release agent 14 measured at the midpoint C1.
[0085] According to at least one of the embodiments described above, it is possible to provide a ceramic substrate, a ceramic circuit board, a semiconductor device, a method for producing a slurry, and a method for applying a release agent, which have high yields even when the components of the release agent 14 are contained.
[0086] Although several embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be embodied in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included within the scope and spirit of the invention, and are also included in the scope of the invention and its equivalents as defined in the claims.
Claims
1. A ceramic substrate having a first surface and a second surface on the front and back sides, wherein when a midpoint C1 is defined as a midpoint of a line segment connecting a center P1 of the first surface and a center P2 of the second surface, the amount of a release agent component measured at the center P1 of the first surface or the center P2 of the second surface is 5 times or more the amount of the release agent component measured at the midpoint C1.
2. The ceramic substrate according to claim 1, characterized in that the ratio P1 / P2 of the amount of the release agent measured at the center P1 of the first surface to the amount of the release agent measured at the center P2 of the second surface satisfies 0.5≦P1 / P2≦2.
3. The ceramic substrate according to claim 1, characterized in that the amount of the release agent component measured at the midpoint C1 is greater than 0 ppm by mass and not more than 50 ppm by mass.
4. The ceramic substrate according to claim 2, characterized in that the amount of the release agent component measured at the midpoint C1 is greater than 0 ppm by mass and not more than 50 ppm by mass.
5. The ceramic substrate according to claim 1, wherein the component of said release agent is boron nitride.
6. The ceramic substrate according to claim 4, wherein the component of said release agent is boron nitride.
7. The ceramic substrate according to claim 1, characterized in that the ceramic substrate is mainly composed of nitride ceramics.
8. The ceramic substrate according to claim 4, characterized in that the ceramic substrate is mainly composed of nitride ceramics.
9. The ceramic substrate according to claim 6, characterized in that the ceramic substrate is mainly composed of nitride ceramics.
10. A ceramic circuit board using the ceramic substrate according to claim 1, characterized in that at least one conductor portion is bonded to at least one of the first surface and the second surface of the ceramic substrate.
11. A ceramic circuit board using the ceramic substrate according to claim 4, characterized in that at least one conductor portion is bonded to at least one of the first surface and the second surface of the ceramic substrate.
12. A ceramic circuit board using the ceramic substrate according to claim 9, characterized in that at least one conductor portion is bonded to at least one of the first surface and the second surface of the ceramic substrate.
13. A ceramic circuit board as described in claim 10, characterized in that the ceramic substrate and the conductor portion are joined via a brazing material, the brazing material contains at least an active metal, and the brazing material contains at least one metal component selected from Ag, Al, Cu, Sn, In and Mn as a metal component other than the active metal.
14. A ceramic circuit board as described in claim 12, characterized in that the ceramic substrate and the conductor portion are joined via a brazing material, the brazing material contains at least an active metal, and the brazing material contains at least one metal component selected from Ag, Al, Cu, Sn, In and Mn as a metal component other than the active metal.
15. The ceramic circuit board according to claim 14, wherein the active metal is at least one selected from the group consisting of Ti, Zr, Nb and Hf.
16. A semiconductor device comprising the ceramic circuit board according to claim 10 and a semiconductor element disposed thereon.
17. A method for producing a slurry, comprising: a washing step of washing ceramic sintered pieces to obtain ceramic sintered pieces from which a portion of the release agent has been separated; and a mixing step of adding the ceramic sintered pieces from which a portion of the release agent has been separated to the new slurry in an amount of 25% by mass or less, when the powder raw material of the new slurry is taken as 100% by mass, and mixing the new slurry to obtain a regenerated slurry.
18. A method for applying a release agent, comprising: a washing step of washing a ceramic sintered piece to obtain a ceramic sintered piece from which a portion of the release agent has been separated; an adjustment step of adjusting the content of the separated release agent to obtain a solution containing the release agent; a dispersion step of uniformly dispersing the concentration of the release agent contained in the solution adjusted by the adjustment step; and a coating step of coating the solution that has been subjected to the dispersion step onto a sheet-shaped ceramic molded body.
Citation Information
Patent Citations
Silicon nitride substrate and method for manufacturing a silicon nitride substrate
JP5673847B2
Release agent recycling device
CN209554904U
Circuit base plate for power module and its production
JP1998067586A
Al / AlN JOINT MATERIAL, BASE PLATE FOR POWER MODULE, POWER MODULE AND PROCESS FOR PRODUCING Al / AlN JOINT MATERIAL
WO2005098942A1
Silicon nitride substrate production method and silicon nitride substrate
WO2020090832A1
Cited By
Cleaning apparatus, cleaning system, cleaning method, and reuse method
JP2026174051A