Hard-coat film and method for manufacturing same

The hard coat film with an ionizing radiation-curable resin composition on both sides of a base film, treated at specific temperatures, addresses the challenges of heat resistance and optical properties, ensuring stability and flexibility, and preventing deterioration in appearance and shape change.

WO2024203972A1PCT designated stage expired Publication Date: 2024-10-03NIPPON PAPER IND CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011527
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-26
Filing Date
2024-03-23
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing hard coat films for flat panel displays and flexible substrates lack sufficient heat resistance, dimensional stability, and optical properties, leading to deterioration in appearance and shape change after heat treatment, while also requiring improved scratch resistance and flexibility.

Method used

A hard coat film with a hard coat layer containing an ionizing radiation-curable resin composition on both sides of a base film, comprising an acrylic resin with (meth)acryloyl groups and inorganic or organic fine particles, which is heat-treated at 150 to 200°C to achieve a maximum thermal shrinkage rate of 1.2% or less and Δ haze of 1.0% or less, ensuring flexibility and maintaining optical properties.

Benefits of technology

The hard coat film achieves high heat resistance, dimensional stability, and flexibility, suppressing appearance and shape changes after heat treatment, while maintaining excellent optical properties and scratch resistance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a hard coat film having high heat resistance or dimensional stability and excellent optical characteristics or flexibility. In this hard coat film, a hard coat layer containing an ionizing-radiation-curable resin composition is provided on both surfaces of a base material film, and the hard coat film satisfies conditions (I), (II), and (III). (I): The ionizing-radiation-curable resin composition contains an acrylic resin including a (meth)acryloyl group. (II): The ionizing-radiation-curable resin composition contains inorganic fine particles or organic fine particles. (III): The maximum value of the thermal shrinkage after the hard coat film has been heat-treated at 150-200°C for 1-30 minutes is 1.2% or less, and the flexibility is 7 mm or less. (IV): The ∆haze defined by the following formula after the hard coat film has been heat-treated at 150-200°C for 1-30 minutes is within the range of 1.0% or less, and whitening of appearance / deformation does not occur even when heat treatment is performed. ∆Haze (%) = haze after heat treatment – haze before heat treatment
Need to check novelty before this filing date? Find Prior Art

Description

Hard coat film and method for producing the same

[0001] The present invention relates to a hard coat film, and more particularly to a hard coat film provided with a hard coat layer that can be used as a component for flat panel displays such as liquid crystal display devices, plasma display devices, and electroluminescence (EL) display devices, touch panels, and the like, or as a base film for carrier films, flexible substrates, and the like.

[0002] The display surface of a flat panel display such as a liquid crystal display (LCD) is required to be scratch-resistant so as to prevent scratches during handling and reduce visibility. Therefore, scratch resistance is commonly imparted by using a hard-coated film in which a hard-coat layer is provided on a substrate film. Furthermore, with the recent widespread use of touch panels that allow users to input data and instructions by touching the display screen with a finger or pen while viewing the display, there are increasing functional requirements for hard-coated films that suppress whitening of the appearance, have high total light transmittance, and have low haze.

[0003] On the other hand, the needs for base films such as carrier films and flexible substrates have become more complex in recent years, necessitating the development of new materials and technologies to realize new electronics. There is a growing demand for films with excellent heat resistance (dimensional stability) and adhesion to laminated films formed on top of them. Therefore, high-performance films that can meet the demand for even higher performance are required by providing various substrate films with hard coat layers (functional layers) to impart properties not obtainable with the substrate film alone.

[0004] Therefore, polyethylene terephthalate, polyethylene naphthalate, triacetyl cellulose, cycloolefin, which are excellent in transparency, heat resistance, dimensional stability, and low moisture absorption, and polyimide and liquid crystal polymer, which are even more excellent in dimensional stability, are expected to be used as substrate films for optical components and electronic components. With the recent diversification of applications, hard-coated films in which a hard-coat layer is provided on such substrate films to further impart hardness are required to not only have excellent adhesion between the substrate film and the hard-coat layer, but also to have excellent optical properties, heat resistance, and adhesion to laminated films.

[0005] Conventionally, methods for imparting easy adhesion to a hard coat layer to a substrate film such as a cycloolefin film having particularly excellent optical properties have been disclosed in Patent Documents 1 and 2. Patent Document 1 discloses a method of subjecting the surface of the substrate film to corona treatment, plasma treatment, UV treatment, or the like, while Patent Document 2 discloses applying an anchor coating agent to the substrate film (anchor coating treatment).

[0006] JP 2001-147304 A JP 2006-110875 A

[0007] Furthermore, base films for flexible substrates and the like are required to have high heat resistance (dimensional stability) and flexibility. For example, after heat treatment, the film must not deteriorate in appearance, change in shape, or change in optical properties (e.g., haze), and must not crack when bent.

[0008] Therefore, an object of the present invention is to provide a hard coat film that has high heat resistance and dimensional stability, is suppressed from deteriorating in appearance and changing in shape after heat treatment, and is also excellent in optical properties and flexibility, and a method for producing the same.

[0009] As a result of extensive research to solve the above problems, the present inventors have found that, since the hard coating allows for heat treatment at high temperatures, by performing an annealing treatment after the hard coating, a hard-coated film having excellent heat resistance and dimensional stability, as well as excellent optical properties and flexibility, can be obtained.

[0010] That is, the present invention has the following configuration. (First Invention) A hard-coated film having a hard-coat layer containing an ionizing radiation-curable resin composition provided on each side of a substrate film, the hard-coat film being characterized by satisfying the following conditions (I), (II), (III), and (IV). Condition (I): The ionizing radiation-curable resin composition contains an acrylic resin containing a (meth)acryloyl group. Condition (II): The ionizing radiation-curable resin composition contains inorganic or organic fine particles. Condition (III): After the hard-coated film is heat-treated at 150 to 200°C for 1 to 30 minutes, the maximum heat shrinkage is 1.2% or less and the flexibility is 7 mm or less. Condition (IV): After the hard-coated film is heat-treated at 150 to 200°C for 1 to 30 minutes, the Δhaze defined by the following formula is within a range of 1.0% or less, and whitening or deformation does not occur in the appearance even after the heat treatment. Δ haze (%)=(haze of the hard-coated film after heat treatment)−(haze of the hard-coated film before heat treatment)

[0011] (Second Invention) The hard coat film according to the first invention, wherein the content of the inorganic or organic fine particles is in the range of 1 to 60 mass % relative to the solid content of the ionizing radiation curable resin composition.

[0012] (Third Invention) The thickness of the hard coat layer A on one side of the substrate film is D A The thickness of the hard coat layer B on the other side is D B When the thickness of the hard coat layers A and B is A , D B are hard coat films according to the first or second invention, characterized in that the thickness of each of them is in the range of 0.5 to 12.0 μm.

[0013] (Fourth Invention) The thickness of the hard coat layer A on one side of the substrate film is D A The thickness of the hard coat layer B on the other side is D B When the thickness ratio of the hard coat layer A to the hard coat layer B isA / D B )×100) is in the range of 50 to 150%.

[0014] (Fifth Invention) The hard coat film according to the first or second invention, wherein the base film is any film selected from polyethylene terephthalate, cycloolefin, polyethylene naphthalate, polyimide, triacetyl cellulose, and liquid crystal polymer.

[0015] (Sixth Invention) A method for producing a hard coat film having a hard coat layer containing an ionizing radiation curable resin composition provided on each side of a substrate film, the method comprising: coating each side of the substrate film with an ionizing radiation curable resin composition containing an acrylic resin having a (meth)acryloyl group and inorganic or organic fine particles; drying the coated film; and irradiating the coated film with ionizing radiation to form a cured hard coat layer on each side of the substrate film; and annealing the resulting hard coat film.

[0016] (Seventh Invention) The method for producing a hard coat film according to the sixth invention is characterized in that the annealing treatment is carried out at 150 to 200° C. for 0.1 to 40 minutes.

[0017] (Eighth Invention) The method for producing a hard coat film according to the sixth or seventh invention is characterized in that the hard coat film has a Δ haze defined by the following formula in the range of 1.0% or less, and does not suffer from whitening or deformation in appearance even when subjected to the annealing treatment: Δ haze (%) = (haze of the hard coat film after the annealing treatment) - (haze of the hard coat film before the annealing treatment)

[0018] (Ninth Invention) The method for producing a hard coat film according to the sixth or seventh invention is characterized in that the hard coat film satisfies the following conditions (III) and (IV). Condition (III): The hard coat film has a maximum heat shrinkage of 1.2% or less and a flexibility of 7 mm or less after being heat treated at 150 to 200°C for 1 to 30 minutes. Condition (IV): The hard coat film has a Δ haze defined by the following formula of 1.0% or less after being heat treated at 150 to 200°C for 1 to 30 minutes, and the heat treatment does not cause whitening or deformation in appearance. Formula) Δ haze (%) = (haze of the hard coat film after heat treatment) - (haze of the hard coat film before heat treatment)

[0019] (10th Invention) The method for producing a hard coat film according to the 6th or 7th invention, wherein the content of the inorganic or organic fine particles is in the range of 1 to 60 mass % relative to the solid content of the ionizing radiation curable resin composition.

[0020] (11th Invention) The method for producing a hard coat film according to the 6th or 7th invention, wherein the base film is any film selected from polyethylene terephthalate, cycloolefin, polyethylene naphthalate, polyimide, triacetyl cellulose, and liquid crystal polymer.

[0021] According to the present invention, it is possible to provide a hard-coated film that has high heat resistance and dimensional stability, is suppressed from deterioration in appearance and change in shape after heat treatment, and is also excellent in optical properties and flexibility. Furthermore, according to the method for producing a hard-coated film of the present invention, a hard-coated film having the above-mentioned various excellent properties can be obtained, particularly by performing an annealing treatment after hard coating.

[0022] Hereinafter, embodiments for carrying out the present invention will be described in detail, but the present invention is not limited to the following embodiments. In this specification, the expression "xx to yy" as a numerical range means "xx or more and yy or less" unless otherwise specified.

[0023] As described in the first aspect of the present invention, the present invention provides a hard-coated film having a substrate film and a hard-coat layer containing an ionizing radiation-curable resin composition provided on each of the two surfaces thereof, the hard-coated film satisfying the following conditions (I), (II), (III), and (IV): Condition (I): The ionizing radiation-curable resin composition contains an acrylic resin containing a (meth)acryloyl group; Condition (II): The ionizing radiation-curable resin composition contains inorganic or organic fine particles; Condition (III): After the hard-coated film is heat-treated at 150 to 200°C for 1 to 30 minutes, the maximum heat shrinkage is 1.2% or less and the flexibility is 7 mm or less; Condition (IV): After the hard-coated film is heat-treated at 150 to 200°C for 1 to 30 minutes, the Δhaze defined by the following formula is within a range of 1.0% or less, and the hard-coated film does not whiten or deform in appearance even after the heat treatment. Δ haze (%)=(haze of the hard coat film after heat treatment)−(haze of the hard coat film before heat treatment) The structure of the hard coat film of the present invention will be described in detail below.

[0024] [Substrate film] First, the substrate film of the hard coat film of the present invention will be described. In the present invention, the substrate film of the hard coat film is not particularly limited, and examples thereof include films or sheets of polyethylene terephthalate, cycloolefin, polyethylene naphthalate, polyimide, polyethylene, polypropylene, acrylic resin, polystyrene, triacetyl cellulose, polyvinyl chloride, liquid crystal polymer, etc. Among them, it is preferable to use polyethylene terephthalate, cycloolefin, polyethylene naphthalate, polyimide, triacetyl cellulose, liquid crystal polymer, etc., which are excellent in heat resistance and dimensional stability, and among them, it is more preferable to use polyethylene terephthalate, which is inexpensive and easily available, and cycloolefin, which is excellent in optical properties and low moisture absorption.

[0025] In the present invention, the thickness of the substrate film is appropriately selected depending on the application for which the hard coat film is used, but from the viewpoints of mechanical strength, handleability, etc., it is preferably in the range of 10 to 300 μm, more preferably in the range of 20 to 200 μm.

[0026] In the present invention, when the above-mentioned substrate film is used for hard coat film applications, in order to prevent deterioration of the coating film and poor adhesion due to ultraviolet rays, a resin constituting the substrate film and an ultraviolet absorber may be kneaded together to form a film, or a film may be used in which a coating material containing a mixture of a thermoplastic or thermosetting resin and an ultraviolet absorber is applied to one or both sides of the substrate film.

[0027] [Hard Coat Layer] Next, the hard coat layer will be described. In the present invention, the hard coat layer contains an ionizing radiation curable resin composition. The hard coat layer is formed of a cured coating film of this ionizing radiation curable resin composition. As the resin contained in the hard coat layer, it is preferable to use an ionizing radiation curable resin composition, in particular, because it imparts surface hardness (pencil hardness, scratch resistance) to the hard coat layer and also makes it possible to adjust the degree of crosslinking by the amount of ultraviolet light exposure, thereby enabling adjustment of the surface hardness of the hard coat layer.

[0028] In the present invention, the ionizing radiation-curable resin composition contains an acrylic resin containing a (meth)acryloyl group (condition (I) above). The ionizing radiation-curable resin composition used in the present invention is a transparent resin that is cured by irradiation with ultraviolet light (hereinafter abbreviated as "UV") or an electron beam (hereinafter abbreviated as "EB"), and preferably contains an acrylic resin containing a (meth)acryloyl group. In particular, to improve coating hardness and form a three-dimensional crosslinked structure in the hard coat layer, it is preferable to contain a polyfunctional acrylate resin having three or more (meth)acryloyloxy groups in one molecule, and it is even more preferable to contain a urethane acrylate resin containing a (meth)acryloyl group.

[0029] Specific examples of polyfunctional acrylates having three or more (meth)acryloyl groups in one molecule include urethane acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, trimethylolpropane ethoxy triacrylate, glycerin propoxy triacrylate, ditrimethylolpropane tetraacrylate, etc. The acrylic resin containing a (meth)acryloyl group may be used singly or in combination of two or more acrylic resins.

[0030] As described above, the ionizing radiation curable resin composition used in the present invention further contains inorganic or organic fine particles (condition (II) above). By containing these inorganic or organic fine particles, it is possible to improve the surface hardness (scratch resistance) and surface smoothness of the hard coat layer. Furthermore, as described above, it also contributes to improving the heat resistance of the hard coat film.

[0031] In this case, the average particle size of the inorganic or organic fine particles is preferably in the range of 1 to 500 nm, more preferably in the range of 10 to 100 nm. If the average particle size is less than 1 nm, it is difficult to obtain sufficient surface hardness. On the other hand, if the average particle size exceeds 500 nm, the gloss and transparency of the hard coat layer may decrease, and the flexibility may also decrease.

[0032] Examples of the inorganic or organic fine particles include silica, alumina, acrylic, silicone resin, etc. In the present invention, it is particularly preferable to contain silica, which is an inorganic fine particle that provides an excellent appearance to the hard coat film, has very high binding energy, and is excellent in thermal stability.

[0033] In the present invention, the content of the inorganic or organic fine particles is preferably in the range of 1 to 60% by mass, particularly preferably 15 to 50% by mass, based on the solid content of the ionizing radiation-curable resin composition. If the content is less than 1% by mass, it is difficult to obtain the effects of improving surface hardness (scratch resistance) and heat resistance. On the other hand, if the content exceeds 60% by mass, flexibility decreases and haze increases, which is undesirable.

[0034] Furthermore, in addition to the above-mentioned acrylic resin containing a (meth)acryloyl group, the ionizing radiation curable resin composition may contain thermoplastic resins such as polyethylene, polypropylene, polystyrene, polycarbonate, polyester, styrene-acrylic, and cellulose, and thermosetting resins such as phenolic resins, urea resins, unsaturated polyesters, epoxy resins, and silicone resins, within a range that does not impair the effects of the present invention or the hardness and scratch resistance of the hard coat layer.

[0035] Furthermore, the photopolymerization initiator for the ionizing radiation-curable resin composition is not particularly limited, and commercially available acetophenones such as Omnirad 651 and Omnirad 184 (both trade names: manufactured by IMG) or benzophenones such as Omnirad 500 (trade name: manufactured by IMG) can be used.

[0036] [Hardcoat Film] The hardcoat film of the present invention is a hardcoat film in which a hardcoat layer is formed on each side of a substrate film using an ionizing radiation curable resin composition that satisfies the above-mentioned conditions.

[0037] A leveling agent can be used in the hard coat layer to improve coating properties, and known leveling agents such as fluorine-based, acrylic, siloxane-based, and adducts or mixtures thereof can be used. The blending amount can be in the range of 0.01 to 7 parts by mass per 100 parts by mass of the solid content of the resin in the hard coat layer. In addition, in touch panel applications and the like, when adhesion to an optically transparent resin OCR is required for the purpose of adhesion to a cover glass (CG), transparent conductive member (TSP), liquid crystal module (LCM), etc. of a touch panel terminal, a resin with a high surface free energy (approximately 40 mJ / cm) can be used.2 It is preferable to use an acrylic leveling agent or a fluorine-based leveling agent.

[0038] Other additives that may be added to the hard coat layer, if necessary, include an antifoaming agent, a surface tension adjuster, an antifouling agent, an antioxidant, an antistatic agent, an ultraviolet absorber, a light stabilizer, and the like, within a range that does not impair the effects of the present invention.

[0039] The hard coat layer is formed by coating a coating material prepared by dissolving or dispersing the ionizing radiation-curable resin composition, a photopolymerization initiator, and other additives in a suitable solvent onto the substrate film and drying the coating material. The solvent can be appropriately selected depending on the solubility of the resin to be blended, and any solvent can be used as long as it can uniformly dissolve or disperse at least the solid components (resin, photopolymerization initiator, and other additives). Examples of such solvents include known organic solvents, such as aromatic solvents such as toluene, xylene, and n-heptane; aliphatic solvents such as cyclohexane, methylcyclohexane, and ethylcyclohexane; ester solvents such as methyl acetate, ethyl acetate, propyl acetate, isopropyl acetate, butyl acetate, and methyl lactate; ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; and alcohol solvents such as methanol, ethanol, isopropyl alcohol, and n-propyl alcohol. These solvents can be used alone or in combination.

[0040] The coating method for the hard coat layer is not particularly limited, but may be a known coating method such as gravure coating, microgravure coating, fountain bar coating, slide die coating, slot die coating, spin coating, screen printing, or spray coating, and then dried at a temperature of usually about 50 to 120°C.

[0041] In the present invention, a hard coat layer coating material containing the above-mentioned ionizing radiation-curable resin composition or the like is applied to a substrate film, dried, and then irradiated with ionizing radiation (UV, EB, or the like), thereby causing photopolymerization and obtaining a cured coating film (hard coat layer) with excellent hardness. In particular, a hard coat layer having such hardness (scratch resistance) that it is not easily scratched when rubbed with steel wool is preferred. The amount of ionizing radiation (UV, EB, or the like) irradiated to the dried coating film may be any amount necessary to impart such sufficient hardness to the hard coat layer, and can be appropriately set depending on the type of ionizing radiation-curable resin, etc.

[0042] The hard coat film of the present invention is a hard coat film in which a hard coat layer is provided on each of both sides of a substrate film. The thickness of the hard coat layer is not particularly limited, but the thickness of the hard coat layer A on one side of the substrate film is preferably D A The thickness of the hard coat layer B on the other side is D B When the thickness of the hard coat layers A and B is A , D B are preferably in the range of 0.5 to 12.0 μm, and particularly preferably in the range of 0.5 to 9.0 μm. If the film thickness is less than 0.5 μm, the hard coat layer will not have sufficient rigidity, making it difficult for the hard coat layer to suppress thermal deformation of the substrate film. Furthermore, if the film thickness exceeds 12.0 μm, the rigidity of the hard coat layer will be significantly improved, and the flexibility and crack resistance of the hard coat layer will be significantly reduced, which is undesirable. To maintain a balance between these two, it is more preferable that the film thickness (one side) be in the range of 1.0 to 7.0 μm.

[0043] In addition, the film thickness ratio of the hard coat layer A to the hard coat layer B ((D A / D B ) × 100) is preferably in the range of 50 to 150%, particularly preferably in the range of 80 to 120%. When the film thickness ratio of the hard coat layer A to the hard coat layer B is in the above ratio, curling of the hard coat layers A and B due to shrinkage during curing is preferably offset.

[0044] The hard-coated film of the present invention has a maximum heat shrinkage of 1.2% or less and a flexibility of 7 mm or less after being heat-treated at 150 to 200°C for 1 to 30 minutes (condition (III) above). Furthermore, the hard-coated film of the present invention has a Δhaze defined by the following formula of 1.0% or less after being heat-treated at 150 to 200°C for 1 to 30 minutes, and does not suffer from whitening or deformation in appearance even after the heat treatment (condition (IV) above). Formula) Δhaze (%) = (haze of the hard-coated film after heat treatment) - (haze of the hard-coated film before heat treatment)

[0045] As described above, the hard coat film of the present invention satisfies the above conditions (III) and (IV) and has high heat resistance, dimensional stability, and flexibility. Therefore, in the film after the heat treatment, for example, deterioration of appearance, change in shape, etc. are suppressed, and changes in optical properties (e.g., haze, etc.) are also suppressed, and cracks, etc. do not occur when the film is bent.

[0046] [Hard Coat Film Manufacturing Method] The present invention also provides a method for manufacturing a hard coat film, which comprises coating both surfaces of the substrate film with an ionizing radiation curable resin composition containing an acrylic resin having a (meth)acryloyl group and inorganic or organic fine particles, drying the coating, and then irradiating the coating with ionizing radiation to form a cured hard coat layer on each surface of the substrate film, and then annealing the resulting hard coat film.

[0047] The ionizing radiation curable resin composition containing the (meth)acryloyl group-containing acrylic resin and inorganic or organic fine particles is as described above.

[0048] As described above, the method for producing a hard-coated film of the present invention is characterized in that after hard coating, i.e., after forming a hard-coat layer on each side of the substrate film, the resulting hard-coated film is subjected to an annealing treatment. Annealing is a method for removing residual stress in a film by heat treatment. By performing the annealing treatment, the molecules are completely crystallized and fixed, improving heat resistance, dimensional stability, etc.

[0049] The annealing treatment is preferably carried out at a high temperature for a short time, preferably at most about 40 minutes. In the present invention, the annealing treatment is preferably carried out at 150 to 200° C. for 0.1 to 40 minutes, particularly 0.1 to 30 minutes.

[0050] The hard coat film has a Δhaze defined by the following formula in the range of 1.0% or less, and does not suffer from whitening or deformation in appearance even when subjected to the annealing treatment: Δhaze (%) = (haze of hard coat film after annealing treatment) - (haze of hard coat film before annealing treatment)

[0051] The hard-coated film obtained by the hard-coated film manufacturing method of the present invention has a maximum heat shrinkage of 1.2% or less and a flexibility of 7 mm or less after being heat-treated at 150 to 200°C for 1 to 30 minutes. Furthermore, the hard-coated film obtained by the hard-coated film manufacturing method of the present invention has a Δ haze defined by the following formula of 1.0% or less after being heat-treated at 150 to 200°C for 1 to 30 minutes, and does not suffer from whitening or deformation in appearance even after heat treatment: Formula) Δ haze (%) = (haze of the hard-coated film after heat treatment) - (haze of the hard-coated film before heat treatment)

[0052] As explained above, the method for producing a hard coat film of the present invention is suitable for producing a hard coat film of the present invention having the above-mentioned various excellent properties.

[0053] As explained in detail above, the present invention provides a hard-coated film having a hard-coat layer containing an ionizing radiation-curable resin composition on each side of a substrate film, the hard-coat film satisfying the above-mentioned conditions (I), (II), (III), and (IV). According to the present invention, it is possible to provide a hard-coated film that has high heat resistance and dimensional stability, is suppressed from deteriorating in appearance and changing in shape after heat treatment, and is also excellent in optical properties and flexibility. Furthermore, according to the hard-coated film manufacturing method of the present invention, a hard-coated film having the above-mentioned various excellent properties can be obtained, particularly by performing an annealing treatment after hard coating.

[0054] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. Comparative examples and reference examples will also be described. Unless otherwise specified, "parts" in the following descriptions represent "parts by mass" and "%" represents "% by mass".

[0055] Example 1 Preparation of Resin Composition 1 for Forming a Hard Coat Layer (Coating for a Hard Coat Layer) An ionizing radiation curable resin composition (containing a total of 23% of urethane acrylate and acrylic ester containing (meth)acryloyl groups, 15% amorphous silica, 2% photopolymerization initiator, and containing 41.7% propylene glycol monomethyl ether, 3.5% methyl isobutyl ketone, 36.7% methyl ethyl ketone, and 18.2% toluene as solvents) to which a fluorine-based leveling agent was added in an amount of 0.1% relative to the resin content was used as the main component, and the solids concentration was adjusted to 28% with a diluent (a mixture of 65% 1-propanol and 35% diacetone alcohol). In this manner, the resin composition 1 for forming a hard coat layer used in this example was prepared.

[0056] [Preparation of Hard Coat Film] A substrate film containing polyethylene terephthalate as the main component (trade name "Cosmoshine A4360", thickness 125 μm, manufactured by Toyobo Co., Ltd.) was used as the substrate film. The above-mentioned resin composition 1 for forming a hard coat layer was coated on both sides of this substrate film using a bar coater, and the coated film was dried with hot air in a drying oven at 80°C for 1 minute to form a coating layer with a coating thickness of 3.0 μm (one side). The coating thickness was the same on both sides. The coating thickness was measured using a Thin-Film Analyzer F20 (trade name) (manufactured by FILMETRICS). This was irradiated with a UV irradiation device set at a height of 60 mm from the coated surface, with a UV irradiation dose of 193 mJ / cm. 2 The resulting hard-coated film was then heat-treated in a drying oven at 150 to 200°C for 1 to 30 minutes to obtain an annealed hard-coated film. The specific annealing conditions were as shown in Table 1.

[0057] Comparative Example 1 In the same manner as in Example 1, a hard coat layer was formed on each side of the above-mentioned substrate film, and an unannealed hard coat film was produced by omitting the subsequent annealing treatment.

[0058] Comparative Example 2 A hard coat film was produced by forming a hard coat layer on each side of the above substrate film, which had been annealed for 1 to 30 minutes in a drying oven at 150 to 200° C. The specific annealing conditions for the substrate film were the four conditions shown in Table 1.

[0059] Reference Example 1 As Reference Example 1, the following evaluation was also carried out on the substrate film (trade name "Cosmoshine A4360", thickness 125 μm, manufactured by Toyobo Co., Ltd.) containing polyethylene terephthalate as the main component, which was used in the above Examples and Comparative Examples.

[0060] (Reference Example 2) In Reference Example 2, the substrate film of Reference Example 1 was annealed in a drying oven at 150 to 200°C for 1 to 30 minutes to prepare a substrate film, and the following evaluations were performed. The specific annealing conditions for the substrate film were the four conditions shown in Table 1.

[0061] <Evaluation Method> The hard coat films obtained in the above Examples and Comparative Examples, and the substrate film in the Reference Example were evaluated according to the following methods and criteria. The results are summarized in Table 1.

[0062] (1) Optical Properties (Transmittance (Tt), Haze, ΔHaze) Measurements were made using a haze meter HM150 (manufactured by Murakami Color Research Laboratory Co., Ltd.) in accordance with JIS-K-7361-1 and JIS-K-7136. Measurements were made for each film before and after heat treatment (heat treatment at 150°C for 30 minutes and at 200°C for 30 minutes). The ΔHaze defined by the following formula 1 is also shown in the "Optical Properties After Each Heat Treatment" column in Table 1. Formula 1) ΔHaze (%) = (Haze of hard coat film or base film after heat treatment) - (Haze of hard coat film or base film before heat treatment) For each of the films of Example 1 and Reference Example 2 that were subjected to the annealing treatment, the ΔHaze defined by the following formula 2 is also shown in the "Optical Properties" column in Table 1. Δ haze (%) = (haze of hard coat film or base film after annealing) - (haze of hard coat film or base film before annealing) Equation 2) Furthermore, for each film of Comparative Example 2 (Nos. 11 to 14), the formula is shown in Table 1 as Δ haze (%) = (haze of hard coat film after annealing (value after annealing + coating)) - (haze of base film before annealing).

[0063] (2) Heat shrinkage was measured using a small digital measuring microscope (manufactured by Olympus Corporation) in accordance with JIS-K-7133. Each film was heated at 150°C for 30 minutes and at 200°C for 30 minutes. The heat shrinkage was measured in the coating direction of the hard coat film (abbreviated as "MD") and in the width direction (abbreviated as "TD") perpendicular to the coating direction. In the case of the base film of the reference example, the direction in which the molten resin flows during film formation (machine direction) is defined as MD, and the direction perpendicular to the flow direction is defined as TD (transverse direction).

[0064] (3) Flexibility In accordance with the mandrel method of JIS-K-5600-1, a cylindrical mandrel bending tester (manufactured by Allgood Co., Ltd.) was used to measure the minimum diameter (φmm) at which no cracks occurred in the hard coat when the film was bent. The measurements were taken when the film was bent to both the front (one side) side and the back (other side). The smaller the value, the better the flexibility. In particular, a measured value of 5 mm or less indicates excellent flexibility.

[0065] (4) Scratch Resistance: Each hard-coated film was tested in accordance with JIS-K-5600-5 by applying a load of 250 gf / cm to the hard-coat layer surface using steel wool #0000. 2 The film was rubbed back and forth 10 times, and the degree of scratching was evaluated according to the following criteria. Measurements were made on the hard coat layer surfaces of the front (one side) and back (other side) of the film. Products rated A and A' were considered to pass the scratch resistance test. A: No scratches. A': A few scratches (1 to 10 lines). B: 11 to 20 scratches. C: Numerous scratches (21 or more lines).

[0066] (5) Appearance Evaluation The appearances of each film (degree of whitening of the film surface, degree of precipitation of oligomer components from inside the base film, deformation, etc.) before and after the above-mentioned heat treatment (heat treatment at 150°C for 30 minutes and at 200°C for 30 minutes) were visually compared and evaluated. The evaluation criteria are as follows: ○: No change ×: Whitening and deformation

[0067]

[0068] As is clear from the results in Table 1, the hard-coated films of the examples of the present invention satisfy the conditions (I), (II), (III), and (IV) of the present invention and have high heat resistance, dimensional stability, and flexibility. Therefore, in the films after the heat treatment, for example, deterioration in appearance and shape change are suppressed, and changes in optical properties (transmittance, haze, etc.) are also suppressed. That is, according to the present invention, hard-coated films are obtained that have high heat resistance and dimensional stability, are suppressed from deterioration in appearance and shape change after heat treatment, and also have excellent optical properties and flexibility. Furthermore, the hard-coated film manufacturing method of the present invention, in which annealing is performed after hard coating, is suitable for manufacturing the hard-coated films of the present invention that have the various excellent properties described above. On the other hand, the hard-coated films of Comparative Example 1, which is not annealed, and Comparative Example 2, which is hard-coated after annealing, do not satisfy all of the conditions (I), (II), (III), and (IV) of the present invention, and therefore do not obtain hard-coated films that satisfy all of the high heat resistance, dimensional stability, appearance after heat treatment, optical properties, and flexibility. Furthermore, whitening and deformation were observed in the reference examples.

Claims

1. A hard-coat film comprising a hard-coat layer containing an ionizing radiation curable resin composition on each side of a substrate film, the hard-coat film being characterized by satisfying the following conditions (I), (II), (III) and (IV). Condition (I): The ionizing radiation curable resin composition contains an acrylic resin containing a (meth)acryloyl group. Condition (II): The ionizing radiation curable resin composition contains inorganic or organic fine particles. Condition (III): The hard-coat film has a maximum heat shrinkage of 1.2% or less and a bending strength of 7 mm or less after heat treatment at 150 to 200°C for 1 to 30 minutes. Condition (IV): The hard-coat film has a Δ haze defined by the following formula of 1.0% or less after heat treatment at 150 to 200°C for 1 to 30 minutes, and does not whiten or deform in appearance even after heat treatment. Formula) Δ haze (%) = (haze of the hard-coat film after heat treatment) - (haze of the hard-coat film before heat treatment) 2. The hard coat film according to claim 1, characterized in that the content of the inorganic or organic fine particles is in the range of 1 to 60 mass % relative to the solid content of the ionizing radiation curable resin composition.

3. The thickness of the hard coat layer A on one side of the substrate film is set to D. A The thickness of the hard coat layer B on the other surface is D B When the thickness of the hard coat layers A and B is D A , D B and , each of which is in the range of 0.5 to 12.0 μm.

4. The thickness of the hard coat layer A on one side of the substrate film is set to D. A The thickness of the hard coat layer B on the other surface is D B When the thickness ratio of the hard coat layer A to the hard coat layer B ((D A / D B 3. The hard coat film according to claim 1, wherein the ratio of the refractive index to the refractive index of the hard coat film is 50 to 150%.

5. The hard coat film according to claim 1 or 2, characterized in that the base film is any film selected from the group consisting of polyethylene terephthalate, cycloolefin, polyethylene naphthalate, polyimide, triacetyl cellulose, and liquid crystal polymer.

6. A method for producing a hard coat film having a hard coat layer containing an ionizing radiation curable resin composition on both sides of a base film, the method comprising: coating both sides of the base film with an ionizing radiation curable resin composition containing an acrylic resin containing a (meth)acryloyl group and inorganic or organic fine particles; drying the coating, and then irradiating the coating with ionizing radiation to form a cured hard coat layer on each side of the base film; and annealing the resulting hard coat film.

7. The method for producing a hard coat film according to claim 6, wherein the annealing treatment is carried out at 150 to 200° C. for 0.1 to 40 minutes.

8. The method for producing a hard coat film according to claim 6 or 7, characterized in that the hard coat film has a Δhaze defined by the following formula within the range of 1.0% or less, and does not suffer from whitening or deformation in appearance even when the annealing treatment is performed. Formula) Δhaze (%) = (haze of the hard coat film after the annealing treatment) - (haze of the hard coat film before the annealing treatment) 9. The method for producing a hard coat film according to claim 6 or 7, characterized in that the hard coat film satisfies the following conditions (III) and (IV). Condition (III): The hard coat film has a maximum heat shrinkage of 1.2% or less and a bending strength of 7 mm or less after heat treatment at 150 to 200°C for 1 to 30 minutes. Condition (IV): The hard coat film has a Δ haze defined by the following formula of 1.0% or less after heat treatment at 150 to 200°C for 1 to 30 minutes, and does not whiten or deform in appearance even after heat treatment. Formula) Δ haze (%) = (haze of the hard coat film after heat treatment) - (haze of the hard coat film before heat treatment) 10. A method for producing a hard coat film as described in claim 6 or 7, characterized in that the content of the inorganic or organic fine particles is in the range of 1 to 60 mass % relative to the solid content of the ionizing radiation curable resin composition.

11. The method for producing a hard coat film according to claim 6 or 7, characterized in that the base film is any film selected from the group consisting of polyethylene terephthalate, cycloolefin, polyethylene naphthalate, polyimide, triacetyl cellulose, and liquid crystal polymer.

Citation Information

Patent Citations

  • Hard coat film

    JP2020157592A

  • Hard coat film, and manufacturing method thereof

    JP2020157693A

  • Base material for gas-barrier films, gas-barrier film, member for electronic devices, and electronic device

    WO2019078069A1

  • Polyester film and use thereof

    WO2021182191A1

  • Hard coat film

    WO2022210769A1