Flexible metal-clad laminate and method for manufacturing same
The flexible metal-clad laminate, featuring a liquid crystal polymer insulating layer with specific copper foil surface characteristics and a tailored manufacturing process, addresses the challenge of achieving high peel strength and stability for high-frequency applications, ensuring reliable performance in 5G communication equipment.
Patent Information
- Application Number
- PCT/JP2024/011538
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-03
AI Technical Summary
Flexible metal-clad laminates used in high-frequency communication equipment face challenges in achieving sufficient peel strength and dimensional stability, particularly with low-roughness copper foils, which are essential for handling high-frequency bands like 5G.
A flexible metal-clad laminate is developed using a liquid crystal polymer insulating layer with a copper foil having a surface peak density (Spd) between 30.0×10^4 and 49.0×10^4 mm^-2, and a manufacturing method involving hot-press molding with a double belt press device at temperatures 15°C to 30°C higher than the melting point of the polymer, and pressures of 0.5 to 5.5 MPa for 70 to 280 seconds, ensuring high peel strength and minimal dimensional change.
The solution provides a flexible metal-clad laminate with excellent adhesion and electrical properties, maintaining a peel strength of 0.7 N/mm or more and a dimensional change rate within ±0.15%, suitable for high-frequency applications like 5G devices.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure 00000017_0000
Abstract
Description
Flexible metal-clad laminate and manufacturing method thereof
[0001] The present invention relates to a flexible metal-clad laminate and a method for manufacturing the same.
[0002] In recent years, amid calls for the promotion of DX (Digital Transformation), typified by the use of IoT (Internet of Things) and AI, there is a demand for the widespread adoption of 5G, which utilizes high frequency bands such as millimeter waves and sub-6, in order to utilize the vast amounts of data. For this reason, printed wiring boards mounted on communication devices are required to have low transmission loss even in high frequency bands, as well as adhesion and dimensional stability equivalent to conventional products.
[0003] Liquid crystal polymer resins are known for their high heat resistance, low dielectric constant, and low dielectric loss tangent, and flexible printed wiring boards compatible with high-frequency bands, including an insulating layer made of liquid crystal polymer, have been actively used in recent years. Patent Document 1 discloses a method for continuously thermo-compressing a liquid crystal polymer while applying surface pressure using a double-belt press equipped with a pair of endless belts. The metal foil used in this process is copper-plated to a surface roughness Rz of 0.5 to 4.0 μm to ensure sufficient adhesion with the insulating layer, the liquid crystal polymer.
[0004] However, in the copper foil examples disclosed in Patent Document 1, even if the Rz is within the above range, sufficient peel strength is not obtained without copper plating treatment (Example 7, Table 1).
[0005] Patent No. 5411656
[0006] Therefore, the inventors have aimed to provide a flexible metal-clad laminate of liquid crystal polymer with excellent adhesion (peel resistance) and electrical properties by examining the copper foil surface structure from the perspective of area analysis rather than line analysis for metal foil, particularly low-roughness copper foil, that can handle high-frequency bands associated with the shift to high-frequency (5G) electronic devices such as smartphones, and have also conducted intensive research into a method for producing the same.
[0007] The inventors performed a surface structure analysis of the copper foil surface and calculated the peak density Spd, that is, the number of bumps (protrusions) per unit area on the copper foil surface (unit: mm -2 ) is related to adhesiveness (adhesion), and this led to the completion of the present invention. That is, the present invention provides the following inventions [1] to [5]. [1] A flexible metal-clad laminate comprising an insulating layer made of a liquid crystal polymer and a metal layer formed on one or both sides of the insulating layer, wherein the surface of the metal layer that overlaps with the insulating layer has a peak density Spd (mm -2 ) is 30.0 x 10 4 mm -2 Above 49.0 x 10 4 mm -2 [2] A flexible metal-clad laminate according to [1] above, wherein the peel strength between the metal layer and the insulating layer measured by Method A in accordance with JIS C6471:1995 is 0.7 N / mm or more, and the dimensional change rate of the insulating layer measured on a sample prepared by punching a test piece measuring 200 mm in MD x 160 mm in TD with 1 mm diameter gauge marks at 37.5 mm intervals in both MD and TD along the outer periphery of a 150 mm x 150 mm square is within ±0.15%, in accordance with the dimensional stability test specified in JIS C6471:1995. [3] A method for producing a flexible metal-clad laminate, which comprises laminating an insulating layer made of a liquid crystal polymer and a metal layer on one or both sides of the insulating layer and thermocompressing the laminate, and wherein the peak density Spd (mm) of the metal layer on the surface overlapping the insulating layer is measured in accordance with ISO 25178-2:2021. -2 ) is 30.0 x 10 4 mm -2 Above 49.0 x 10 4 mm -2[4] The method for producing a flexible metal-clad laminate according to [3] above, wherein the heating temperature during the thermo-compression molding is in the range of 15°C higher than the melting point of the liquid crystal polymer of the insulating layer to 30°C higher than the melting point. [5] The method for producing a flexible metal-clad laminate according to [3] above, wherein the thermo-compression molding is performed using a double belt press, the pressure during the thermo-compression molding is in the range of 0.5 to 5.5 MPa, and the heating and pressurizing time is in the range of 70 to 280 seconds. [6] The method for producing a flexible metal-clad laminate according to [3] above or [4] above, wherein the metal layer is copper foil.
[0008] According to the present invention, it is possible to provide an excellent flexible metal-clad laminate of a liquid crystal polymer that has excellent adhesive (peel resistance) and electrical properties and a small rate of dimensional change, and a method for producing the same.
[0009] 1 is a schematic diagram showing a schematic configuration of an example of a thermocompression bonding step in a method for producing a flexible metal-clad laminate according to the present invention, and FIG. 2 is an explanatory diagram of a test sample for measuring the dimensional change rate of the flexible copper-clad laminate obtained by etching the copper foil of the flexible copper-clad laminate according to the present invention.
[0010] Preferred embodiments of the present invention will now be described.
[0011] The flexible metal-clad laminate of the present invention is a flexible metal-clad laminate comprising an insulating layer made of a liquid crystal polymer and a metal layer formed on one or both sides of the insulating layer, wherein the surface of the metal layer that overlaps the insulating layer has a peak density Spd (mm -2 ) is 30.0 x 10 4 mm -2 Above 49.0 x 10 4 mm -2 The peel strength between the metal layer and the insulating layer measured by Method A in accordance with JIS C6471:1995 is 0.7 N / mm or more, and the dimensional change rate of the insulating layer measured on a sample prepared by punching a test piece of 200 mm in MD x 160 mm in TD with 1 mm diameter reference marks at 37.5 mm intervals in both MD and TD along the outer periphery of a 150 mm x 150 mm square is within ±0.15%, in accordance with the dimensional stability test specified in JIS C6471:1995.
[0012] <Insulating Layer> In the flexible metal-clad laminate of the present invention, the insulating layer is formed of a liquid crystal polymer. The type of liquid crystal polymer is not particularly limited, and examples include liquid crystal polymers having ethylene terephthalate and parahydroxybenzoic acid as structural units, liquid crystal polymers having phenol, phthalic acid, and parahydroxybenzoic acid as structural units, and liquid crystal polymers having 6-hydroxy-2-naphthoic acid and parahydroxybenzoic acid as structural units. Liquid crystal polymers having 6-hydroxy-2-naphthoic acid and parahydroxybenzoic acid as structural units and liquid crystal polymers having 6-hydroxy-2-naphthoic acid and terephthalic acid as structural units are preferred. In the present invention, the insulating layer may be in either a film or sheet form. The difference between "film" and "sheet" in the present invention is in accordance with the JIS "Packaging Terminology" standard, in which a film is defined as a "plastic film having a thickness of less than 250 μm" and a sheet is defined as a "thin plastic plate having a thickness of 250 μm or more." Methods for forming a film- or sheet-like insulating layer include the T-die method, inflation method, etc. Among these, the inflation method is preferred from the viewpoints of dimensional stability, production costs, etc.
[0013] The thickness of the insulating layer is not particularly limited, and is preferably in the range of, for example, 6 to 300 μm. When an insulating film is used, the thickness is preferably in the range of, for example, 6 μm or more and less than 250 μm, more preferably in the range of 12 to 150 μm, and even more preferably in the range of 25 to 100 μm.
[0014] <Metal Layer> The material of the metal layer constituting the flexible metal-clad laminate of the present invention is not particularly limited as long as it is a metal, and copper, copper alloy, aluminum, stainless steel, etc. are used. Copper and copper alloy are preferred, and copper is more preferred. The form of the metal layer is preferably a metal foil, which can be selected from metal foils of the above materials, and copper foil is particularly preferred.
[0015] In the present invention, the surface of the metal layer overlapping the insulating layer has a peak density Spd (mm -2 ) is 30.0 x 10 4 mm -2 The above is required.
[0016] In the present invention, the "peak density Spd" of the metal layer is a parameter representing the number of peaks per unit area measured in accordance with ISO 25178-2:2021. 2 A large value indicates a large number of contact points with other objects. The peak density Spd is the number of peaks per unit area of a given measurement area (e.g., 100 μm) on the treated surface. 2 In the present invention, the peak density Spd can be calculated by measuring the surface profile of the surface of the surface (region) using a commercially available laser microscope. 2 300,000 pieces per (30.0 x 10 4 ) or more 490,000 pieces (49.0×10 4 ) or less. Preferably, it is 330,000 (33 × 10 4 ) or more, with the upper limit being 430,000 (43.0 x 10 4 ) or less, and 380,000 (38.0 × 10 4 ) The following is even more preferred.
[0017] Furthermore, in the present invention, the surface roughness (ten-point average roughness) Rz of the surface of the metal layer overlapping the insulating layer, as defined in JIS B0601:1994, is preferably in the range of 0.5 to 4.0 μm. A surface roughness Rz in this range, combined with the other surface characteristics described above, is preferable from the viewpoint of ensuring adhesion (adhesion) with a sufficiently high peel strength between the insulating layer and the metal layer. Note that the "adhesion (adhesion)" between the insulating layer and the metal layer in the present invention is based on the strength of the peel strength between the two layers, and is not based on the concept of adhesive strength based on the narrower mode of adhesion, such as "adhesion by chemical bonding."
[0018] The flexible metal-clad laminate of the present invention has a metal layer on one or both sides of an insulating layer. That is, either of the layer structure of embodiment 1, which is metal layer / insulating layer / metal layer, and embodiment 2, which is two layers, which is metal layer / insulating layer, can be selected depending on the application.
[0019] The flexible metal-clad laminate of the present invention is required to have a peel strength between the metal layer and the insulating layer of 0.7 N / mm or more, as measured by Method A in accordance with JIS C6471:1995. It is more preferably 0.8 N / mm or more, and even more preferably 1.0 N / mm or more. If the peel strength between the metal layer and the insulating layer is 0.7 N / mm or more, peel resistance can be ensured when the flexible metal-clad laminate is mounted on a substrate.
[0020] Furthermore, the flexible metal-clad laminate of the present invention is required to have a dimensional change rate of the insulating layer within ±0.15% when measured on a sample prepared by punching a test piece measuring 200 mm in MD x 160 mm in TD with 1 mm diameter gauge marks at 37.5 mm intervals in both MD and TD along the outer periphery of a 150 mm x 150 mm square, in accordance with the dimensional stability test specified in JIS C6471:1995.
[0021] The method for producing a flexible metal-clad laminate of the present invention will be described below. The method for producing a flexible metal-clad laminate of the present invention is a method for producing a flexible metal-clad laminate by overlaying an insulating layer made of a liquid crystal polymer and a metal layer on one or both sides of the insulating layer and thermocompressing the laminate. The method is characterized in that the peak density Spd (mm ) of the metal layer on the surface overlapping the insulating layer is measured in accordance with ISO 25178-2:2021. -2 ) is 30.0 x 10 4 mm -2 Above 49.0 x 10 4 mm -2 The heating temperature during the thermocompression molding is in the range of a temperature 15° C. higher than the melting point of the liquid crystal polymer of the insulating layer to a temperature 30° C. higher than the melting point.
[0022] The liquid crystal polymer and metal layer forming the insulating layer used in the manufacturing method of the present invention are those already described. The "peak density Spd (mm)" measured by a specific method on the surface of the metal layer overlapping the insulating layer is -2 Regarding the "(1)" method, a material that satisfies the values already described is selected and used from the viewpoint of providing an excellent flexible metal-clad laminate of a liquid crystal polymer with a small dimensional change rate while maintaining a sufficiently high peel strength between the insulating layer and the metal layer. Furthermore, the heating temperature during thermocompression molding must be in the range of 15°C higher than the melting point of the liquid crystal polymer of the insulating layer and 30°C higher than the melting point in order to improve the adhesion (adhesion) between the metal layer and the insulating layer, ensure sufficient peel strength, and minimize the dimensional change rate. Preferably, the heating temperature is in the range of 17°C higher than the melting point and 27°C higher than the melting point. If the heating temperature is below the melting point, the peel strength between the metal layer and the insulating layer is weak, and there is a concern that the circuit may peel off when the flexible metal-clad laminate is processed into a flexible circuit board.
[0023] In the method for producing a flexible metal-clad laminate of the present invention, the method of thermo-pressing may be either a method using a thermo-press roll or a method using a double belt press device for thermo-pressing between endless belts, as long as the method ensures the adhesion (tightness) between the metal layer and the insulating layer and the functionality of the metal-clad laminate. However, it is particularly preferable to perform the thermo-pressing using a double belt press device, from the viewpoint of being able to ensure continuous heating and pressing time while suppressing misalignment between the metal layer and the insulating layer when they are overlapped.
[0024] In the case of embodiment 2, in which the thermocompression molding is performed using a double-belt press, a flexible metal-clad laminate having a metal layer on only one side of the insulating layer is produced. To prevent the steel belt from being transferred to the softened insulating layer (film) during the thermocompression molding process, a release film may be superimposed on the insulating layer (film) to produce a release film / insulating layer / metal layer structure. As the release film, a known release film used in the manufacture of flexible metal-clad laminates can be used. In particular, it is preferable to use a release film made of a flexible material with high heat resistance and good releasability, such as at least one material selected from non-thermocompression-bondable heat-resistant aromatic polyimides, fluororesins, and silicone resins. The release film is appropriately peeled off when the flexible metal-clad laminate is used. In addition, in Figure 1, the metal foil 12 on the upper side can be replaced with a release film (not shown), and after running it through the double belt press device 20, a recovery roll for recovering the release film can be separately provided in the winding section 40, and the release film can be peeled off from the flexible metal-clad laminate 10 at the time it is transported out of the double belt press device 20, and the flexible metal-clad laminate 10 and the release film can be recovered separately.
[0025] In the manufacturing method of the present invention, the pressure applied during thermocompression molding may be set as appropriate, but is preferably in the range of 0.5 to 5.5 MPa, more preferably 2.0 to 5.0 MPa, and even more preferably 3.0 to 4.5 MPa. Setting the pressure applied during thermocompression molding within these ranges allows high peel strength to be maintained. Furthermore, in the manufacturing method of the present invention, the heating and pressurizing time during thermocompression molding may be set as appropriate, but is preferably in the range of 70 to 280 seconds, more preferably 80 to 240 seconds, and even more preferably 90 to 180 seconds. Within these ranges, the dimensional stability of the insulating layer can be improved.
[0026] EXAMPLES The present invention will be described below with reference to examples and comparative examples, but the present invention is not limited to these examples.
[0027] The following materials were prepared and used in the Examples and Comparative Examples. Liquid crystal polymer film for insulating layer: LCP1: manufactured by Okura Kogyo Co., Ltd., melting point 318°C LCP2: manufactured by Kuraray Co., Ltd., melting point 310°C Copper foil was used as the metal layer, and the type, thickness, surface roughness, and peak density Spd (mm -2 The manufacturer, grade, type and thickness of the copper foil used as the metal layer in the examples and comparative examples are shown in Table 1.
[0028]
[0029] The surface characteristics of the copper foil used as the metal layer were evaluated using the method described below. Surface analysis (peak density Spd) of the matte copper foil surface (surface overlapping the insulating layer) was performed using a laser microscope (Keyence Corporation, Model VK-X210) at four random points on an A4-sized copper foil cut out. Measurements were performed in accordance with ISO 25178-2:2021, with an S filter of 1 μm, F-operation surface tilt correction automatic, and an L filter of 0.1 mm. The values shown in Table 2 are the average values of the four measured points. Surface roughness (ten-point average roughness) Rz of the matte copper foil surface was measured using the catalog value published by the copper foil manufacturer.
[0030] The peel strength, which is a performance required for the flexible metal (copper) clad laminates obtained in the examples and comparative examples, was measured and evaluated by the method described below. - Evaluation of peel strength Peel strength in normal condition was measured by Method A in accordance with JIS C6471:1995. The conductor width of the test piece was 3 mm. A peel strength of 0.7 N / mm or more and a dimensional change rate after etching measured below within ±0.15% were evaluated as good (○), and other cases were evaluated as poor (×). - Evaluation of dimensional change rate The dimensional change rate after copper foil etching was measured with reference to the dimensional stability test specified in JIS C6471:1995. As shown in FIG. 2 , the test sample 50 was prepared by cutting out a sample of 200 mm in MD × 160 mm in TD from the center in the width direction of a copper-clad laminate (CCL), and punching 1 mm diameter reference marks 51 at 37.5 mm intervals in both MD and TD along the outer periphery of a 150 mm × 150 mm square, a total of 16 points. The copper foil of the sample was then etched with an aqueous ferric chloride solution at 45° C., and the dimensional change rate was measured before and after the etching.
[0031] Example 1 Using a double belt press device 20 having the configuration shown in FIG. 1, a liquid crystal polymer film 11 (manufactured by Okura Kogyo Co., Ltd., melting point 318°C, thickness 50 μm) was used as the insulating film roll 31 suspended on the unwinding section 30, and an electrolytic copper foil (TQ-M7-VSP, thickness 12 μm) manufactured by Mitsui Mining & Smelting Co., Ltd. was used as the metal layer roll 32, with a surface roughness Rz of 1.2 μm and a peak density Spd of 368959 / mm 2The resulting three-layer structure was fed into a double-belt press 20, sandwiched between an endless belt 23 stretched between upper drums 21 and an endless belt 24 stretched between lower drums 22, and passed through the zones of an upper and lower heat press 25. The laminate was heated to 335°C (17°C higher than the melting point of the liquid crystal film), subjected to a pressure of 4.0 MPa, and heated and pressed for 93 seconds to produce a flexible copper-clad laminate 10, which was then wound into a roll by a winding section 40. The resulting flexible copper-clad laminate 10 had a three-layer structure in which metal layers made of copper foils 12, 12 were laminated on top and bottom of an insulating layer made of a liquid crystal polymer film 11. The peel strength was evaluated using the method described above and found to be 0.99 N / mm. The dimensional change rate after etching was -0.08% in the MD direction and -0.13% in the TD direction. Based on these results, the evaluation was good (○). The configuration of the insulating film and metal foil (copper foil), the thermo-compression molding (heating and pressing) conditions, and the evaluation results are summarized in Table 2.
[0032] Examples 2 to 10, Comparative Examples 1 to 4 In Example 9, LCP2 was used as the liquid crystal film for the insulating layer, but the same insulating film LPC1 was used in all other cases. The copper foils with the manufacturer names and grades shown in Table 1 were used for the metal layers in Examples 2 to 10 and Comparative Examples 1 to 4. The heating temperature (thermocompression molding) conditions were as follows: Example 9, a temperature 15°C higher than the melting point; Example 10, a temperature 27°C higher; Comparative Example 3, a temperature 12°C higher; and Comparative Example 4, a temperature 32°C higher than the melting point; and a heating time of 75 seconds. Flexible copper-clad laminates were produced in the same manner as in Example 1. The configuration of the insulating layer and metal (copper) foil, the thermocompression molding (heating and pressing) conditions, the peel strength of the obtained flexible metal-clad laminates, the dimensional change rate after etching, and the evaluation results are summarized in Table 2.
[0033]
[0034] As can be seen from Table 2, Examples 1 to 10 achieved high peel strengths ranging from 0.74 to 1.04 N / mm. In contrast, Comparative Example 1, which had a peak density of 540,000, exceeding the upper limit of the present invention, and Comparative Example 2, which had a peak density of 290,000, below the lower limit of 300,000, exhibited low peel strengths of 0.53 N / mm and 0.13 N / mm. Furthermore, Comparative Example 3 did not meet the heating processing conditions of 330°C, which was 12°C higher than the melting point of the insulating film (318°C), and the requirement of a temperature at least 15°C higher than the melting point specified in the manufacturing method of the present application. The heating and pressing time was 124 seconds, but the dimensional change rate was outside the specified value. Comparative Example 4, which had a heating temperature of 350°C and 32°C, exceeding the upper limit of the specified value of 30°C, exhibited a dimensional change rate that exceeded the specified value. Therefore, it has been demonstrated that the present invention can provide a flexible copper-clad laminate having excellent adhesion (peel resistance) between the insulating layer and the metal layer and a dimensional change rate after etching of within ±0.15%.
[0035] The flexible metal-clad laminate of the present invention has a high peel strength between the metal layer and the insulating layer of 0.7 N / mm or more, and a dimensional change rate after etching of within ±0.15%, so that the flexible metal-clad laminate can be suitably used for flexible printed wiring boards that can be used in high frequency bands. Furthermore, the method for producing a flexible metal-clad laminate of the present invention can be used as a method for producing the flexible metal-clad laminate reproducibly, stably, and economically.
[0036] 10: Flexible metal-clad laminate (flexible copper-clad laminate) 11: Liquid crystal polymer film 12: Metal foil (copper foil) 20: Double belt press device 21: Upper drum 22: Lower drum 23, 24: Endless belts 25: Heat pressing (molding) device 30: Payout section 31: Insulating film roll 32: Metal layer roll 40: Winding section 50: Sample for measuring dimensional change rate 51: φ1 mm gauge
Claims
1. A flexible metal-clad laminate comprising an insulating layer made of a liquid crystal polymer and a metal layer formed on one or both sides of the insulating layer, wherein the surface of the metal layer overlapping the insulating layer has a peak density Spd (mm -2 ) is 30.0 x 10 4 mm -2 Above 49.0 x 10 4 mm -2 a peel strength between the metal layer and the insulating layer measured by Method A in accordance with JIS C6471:1995 of 0.7 N / mm or more, and a dimensional change rate of the insulating layer measured on a sample prepared by punching a total of 16 φ1 mm gauge marks on a 150 mm × 150 mm square outer periphery at 37.5 mm intervals in both MD and TD in a test piece of 200 mm in MD × 160 mm in TD in accordance with the dimensional stability test specified in JIS C6471:1995 is within ±0.15%.
2. The flexible metal clad laminate of claim 1, wherein said metal layer is copper foil.
3. A method for producing a flexible metal-clad laminate comprising: an insulating layer formed of a liquid crystal polymer; and a metal layer on one or both sides of the insulating layer, and then thermocompressing the insulating layer; wherein the peak density Spd (mm -2 ) is 30.0 x 10 4 mm -2 Above 49.0 x 10 4 mm -2 the heating temperature during the thermocompression molding is in the range of 15° C. higher than the melting point of the liquid crystal polymer of the insulating layer to 30° C. higher than the melting point.
4. The method for producing a flexible metal-clad laminate according to claim 3, wherein the thermo-compression molding is performed using a double belt press device, the pressure during the thermo-compression molding is in the range of 0.5 to 5.5 MPa, and the heating and pressurizing time is in the range of 70 to 280 seconds.
5. The method for producing a flexible metal-clad laminate according to claim 3 or 4, wherein the metal layer is a copper foil.
Citation Information
Patent Citations
Metal clad laminated plate and method for manufacturing metal clad laminated plate
WO2020090688A1
Surface-treated copper foil, carrier-attached copper foil, copper-clad laminate, and printed wiring board
WO2020105289A1
Double-sided metal-clad laminate and production method therefor, insulating film, and electronic circuit base board
WO2020153391A1