Heat-adhesive laminate
The heat-adhesive laminate with PPSU, PESU, or PSU and a polyolefin-based resin layer addresses the durability and cost issues in fuel cell components by enhancing adhesive strength and recyclability, ensuring long-term performance and cost-effectiveness in hot water environments.
Patent Information
- Application Number
- PCT/JP2024/011553
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-03
AI Technical Summary
Fuel cell components, particularly those using polyethylene naphthalate (PEN) as a core material, face issues with hydrolysis and reduced adhesive strength in high-temperature water, leading to durability concerns and increased material costs due to the use of expensive super engineering plastics like polyphenylsulfone (PPSU), polyethersulfone (PESU), and polysulfone (PSU), which have poor adhesive properties and are difficult to recycle.
A heat-adhesive laminate is developed using a resin base material containing PPSU, PESU, or PSU with a polyolefin-based heat-adhesive resin layer and an active energy ray-curable adhesive composition, including compounds with glycidyl ether groups and epoxy groups, to enhance adhesive strength and durability in hot water environments, while minimizing the use of expensive plastics through a high-speed production method.
The laminate achieves excellent adhesive strength and durability in hot water, extending the life of polymer electrolyte fuel cells and water electrolyzers, while reducing material waste and production costs by utilizing a recyclable and cost-effective approach.
Smart Images

Figure JP2024011553_03102024_PF_FP_ABST
Abstract
Description
Heat-adhesive laminate
[0001] The present invention relates to a heat-adhesive laminate, which can be preferably used as a component of a fuel cell or a water electrolysis device.
[0002] In recent years, fuel cells, which generate electricity using hydrogen as fuel, have been attracting increasing attention amid the social challenge of reducing carbon dioxide emissions against the backdrop of global warming. In particular, efforts to replace automobile engines with fuel cells have been gaining momentum in recent years. Hydrogen can be produced using water and solar energy. For example, hydrogen can be produced by electrolyzing water using electricity generated by solar cells. In recent years, there has also been increased research into water electrolysis devices that use water and electricity in a structure similar to a fuel cell. In this way, solar energy, which fluctuates greatly depending on the season and time, can be stored and transported in the form of chemical energy called hydrogen.
[0003] Solid polymer electrolyte fuel cells have become the most widely used fuel cell for automobiles. Various detailed structural designs have been explored, including one example in which a frame-shaped heat-adhesive sheet is used. A sheet serving as a power generation unit is placed and bonded to the window within the frame, while the periphery is bonded to a conductive separator by heat pressing (see, for example, Patent Document 1). The frame-shaped heat-adhesive sheet comprises a heat-adhesive resin layer that firmly bonds to the metal separator by heat pressing, and a base material (also referred to as a core material) that maintains its size and shape during heating. Examples of core materials include polyethylene naphthalate (hereinafter also referred to as "PEN") and polyethersulfone (PES), which have excellent heat resistance and mechanical strength. Examples of heat-adhesive resin layers include polyolefin resins such as polypropylene.
[0004] The frame-shaped thermal adhesive sheet described above is a three-layer laminate in which a thermal adhesive resin layer is formed on both sides of a core material, but it may also be a five-layer laminate in which an easy-adhesion layer is provided between these layers (for example, Patent Document 2).
[0005] Since fuel cells generate water and their temperature rises to near the boiling point of water, the internal components must be durable enough to maintain the performance required for practical use even when immersed in high-temperature water for a long period of time. However, when PEN, which is exemplified in many patent documents (e.g., Patent Documents 1 to 3), is used as the core material, the PEN hydrolyzes and becomes brittle, resulting in a significant decrease in the adhesive strength between separators that is achieved by using a laminate.
[0006] To solve this problem, it is easy to imagine selecting a substrate material that has both excellent hydrolysis resistance and the heat resistance required for fuel cell applications. Known materials with excellent hydrolysis resistance and heat resistance include polyphenylsulfone (hereinafter also referred to as "PPSU"), polyethersulfone (hereinafter also referred to as "PESU"), and polysulfone (hereinafter also referred to as "PSU").
[0007] PPSU and PSU are exemplified as substrates for laminates used inside fuel cells in Patent Document 4. As mentioned above, PESU is exemplified in Patent Document 1 (referred to as PES in Patent Document 1).
[0008] Patent Document 5 describes a gasket member for a polymer electrolyte fuel cell, which is a laminate having a substrate formed of at least one selected from the group consisting of PPSU, PESU, and PSU and adhesive layers disposed on both sides thereof, and which has a breaking elongation retention rate of 60% or more after being left standing in water at 120° C. for 300 hours. Patent Document 6 describes a gasket member for a polymer electrolyte fuel cell having adhesive layers on both sides of a substrate containing PPSU.
[0009] Japanese Patent Publication No. 2017-103126 Japanese Patent Publication No. 2021-54880 Japanese Patent Publication No. 2019-102370 Japanese Patent Publication No. 2020-198199 Japanese Patent No. 7173419 Japanese Patent No. 7151951
[0010] However, because PPSU, PESU, and PSU are poorly adhesive materials, it has been difficult to achieve sufficient adhesive strength with a thermally adhesive resin layer. It has been particularly difficult to achieve adhesive strength in high-temperature water (e.g., peel strength between metal separators in 95°C water), such as that encountered during fuel cell operation. Furthermore, it has been even more difficult to maintain the required adhesive strength even after immersion in 120°C water for significantly longer than 300 hours, e.g., 1,000 hours. Patent Documents 5 and 6 show examples of forming an anchor coating layer on a substrate (core material) using an isocyanate compound or an aminoethylated acrylic polymer. While these methods have been shown to increase adhesive strength at 25°C, the adhesive strength in 95°C water is unknown. Furthermore, although a durability test (e.g., elongation retention at break) involving 300 hours of immersion in 120°C water has been conducted, the adhesive strength after the immersion test is unknown. Furthermore, it is unclear whether sufficient adhesive strength will be maintained even after immersion in water at 120°C for 1,000 hours, but it is difficult to predict that it will be sufficient because it has a hydrolyzable group in its structure and does not have a particularly hydrophobic structure, etc. As described above, improving the hot water resistance of a laminate that uses PPSU, PESU, or PSU as a base material and has an olefin-based heat-adhesive resin layer on at least one surface can be said to be a problem that needs to be solved by a new invention.
[0011] Another problem is that so-called super engineering plastics (super engineering plastics), such as PPSU, PESU, and PSU, are expensive. Therefore, when used for frame-shaped heat-adhesive sheets inside fuel cells, the cost of discarded material during punching increases. Recycling of materials after the laminate is difficult. When holes are first drilled in the substrate, it is possible to recycle the recovered super engineering plastic, but it is difficult to form a heat-adhesive resin layer with a uniform thickness on the pre-punched substrate. Furthermore, to produce them inexpensively, a high-speed production method must be devised. As described above, another problem was how to produce a frame-shaped heat-adhesive laminate for fuel cells or water electrolysis systems that has significantly improved hot water immersion durability compared to PEN substrates, using a method that allows high-speed production without mass disposal of expensive super engineering plastics. The present invention aims to provide a heat-adhesive laminate that has good adhesion to metal substrates and excellent heat resistance and hydrolysis resistance, specifically, excellent hot water immersion durability.
[0012] As a result of extensive investigations to solve the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by a laminate comprising a resin substrate containing at least one selected from the group consisting of polyphenylsulfone, polyethersulfone, and polysulfone, a polyolefin-based heat-adhesive resin layer, and an adhesive composition for bonding them together, the adhesive composition comprising the following components (A), (B), and (C) as essential components: Component (A): a compound having two or more glycidyl ether groups in one molecule Component (B): a compound having an epoxy group other than component (A) Component (C): a photocationic polymerization initiator The present invention will now be described in detail.
[0013] The heat-adhesive laminate of the present invention has good adhesion to metal substrates and can be made to have extremely excellent hot water immersion durability. Therefore, the life of a polymer electrolyte fuel cell or a water electrolysis device can be significantly improved. Furthermore, the laminate manufacturing method of the present invention can manufacture a heat-adhesive laminate with excellent hot water immersion durability while reducing the amount of expensive super engineering plastics that are discarded.
[0014] Fig. 1 is a diagram showing an example of a cross-sectional view of a laminate of the present invention. Fig. 2 is a diagram showing an example of a step of drilling holes in a resin substrate that are smaller than the holes required for the final product in an example of a method for producing a laminate of the present invention. Fig. 3 is a top view of the vicinity of the punching step in Fig. 2. Fig. 4 is a diagram showing an example of a method for producing a laminate of the present invention. Fig. 5 is a diagram showing an example of a cross-sectional view of an intermediate product after drilling holes in a resin substrate that are smaller than the holes required for the final product, applying an active energy ray-curable adhesive to the adhesive surface of a heat-adhesive resin film, laminating them together, and irradiating them with active energy rays to bond them together. Fig. 6 is a diagram showing an example of a hole drilled in a resin substrate before lamination and a portion punched out after lamination in an example of a method for producing a laminate of the present invention.
[0015] The present invention is as follows: [1] A laminate comprising a resin substrate, a cured product layer of an active energy ray-curable adhesive provided on at least one surface of the resin substrate, and a heat-adhesive resin layer provided on the surface of the cured product layer opposite to the resin substrate, wherein the resin substrate comprises at least one selected from the group consisting of polyphenylsulfone, polyethersulfone, and polysulfone, the heat-adhesive resin layer comprises a polyolefin and / or an acid-modified polyolefin, and the active energy ray-curable adhesive is a composition containing a curable component and component (C): a photocationic polymerization initiator, wherein the curable component comprises the following components (A) and (B) as essential components: component (A): a compound having two or more glycidyl ether groups in one molecule; component (B): a compound having an epoxy group other than component (A), and the contents of components (A) and (B) are 10 to 99% by weight for component (A) and 1 to 90% by weight for component (B), relative to 100% by weight of the total amount of the curable components, A heat-adhesive laminate in which the content of the (C) component is 0.1 to 5 parts by weight per 100 parts by weight of the total amount of curable components. [2] The heat-adhesive laminate according to [1], in which the (A) component contains (a1) a diglycidyl ether of an aliphatic diol having 2 to 10 carbon atoms. [3] The heat-adhesive laminate according to [2], in which the (B) component contains at least one compound selected from the group consisting of (b1) a compound having an alicyclic epoxy group and not an ester skeleton, (b2) a compound having an alicyclic epoxy group and an ester skeleton, and (b3) an epoxidized polybutadiene. [4] The heat-adhesive laminate according to any one of [1] to [3], in which the (b2) component does not account for 50% by weight or more of the total amount of curable components in the active energy ray-curable adhesive (100% by weight). [5] The heat-adhesive laminate according to any one of [1] to [4], in which the active energy ray-curable adhesive further contains an oxetane compound as a curable component. [6] The heat-adhesive laminate according to any one of [1] to [5], which is used as a member of a polymer electrolyte fuel cell or a water electrolysis device.[7] A method for producing a heat-adhesive laminate according to any one of [1] to [5], comprising: (1) a step of subjecting the adhesive surface of the resin substrate and the adhesive surface of a resin film for forming the heat-adhesive resin layer to a corona discharge treatment; and (2) a step of bonding the resin substrate and the resin film with an active energy ray-curable adhesive. [8] A method for producing a heat-adhesive laminate according to [7], further comprising: (3) a step of drilling a hole in the resin substrate before the step (1); and (4) a step of drilling a hole through the heat-adhesive laminate in the hole and its surrounding area after the step (2). The resin substrate, the heat-adhesive resin, the active energy ray-curable adhesive, and the method for producing a heat-adhesive laminate are described in detail below.
[0016] 1. Resin Substrate The resin substrate of the heat-adhesive laminate of the present invention contains at least one selected from the group consisting of polyphenylsulfone (PPSU), polyethersulfone (PESU), and polysulfone (PSU). The resin substrate of the present invention may contain one of these as the main component mixed with other resin components, or may contain additives such as antioxidants, or may be a single resin. From the perspective of material recyclability, a single resin or a material containing only additives uniformly dissolved in the resin is preferred.
[0017] The deflection temperatures under load (ASTM D648, 1.8 MPa) of PPSU, PESU, and PSU are approximately 207°C, 202°C, and 174°C, respectively, which are extremely high heat resistance among thermoplastic resins. Therefore, when these materials are used as the base material of a heat-adhesive laminate, it is possible to prevent the laminate from warping when bonding by hot pressing. In other words, the use of these highly heat-resistant base materials allows the temperature of the heat pressing process to be increased. This increases the adhesive strength between the heat-adhesive resin layer and the metal separator. Furthermore, it also allows the use of materials with high melting points for the heat-adhesive resin layer.
[0018] PPSU, PESU, and PSU are also known to be materials with excellent hydrolysis resistance. This allows them to be sterilized by steam heating, and they are used in medical and food applications. Furthermore, because they have excellent mechanical properties such as impact resistance, they are also used as aircraft materials and sanitary pipes. Their excellent hydrolysis resistance and mechanical properties make them suitable for use as internal materials in polymer electrolyte fuel cells.
[0019] The thickness of the resin substrate may be adjusted according to the specifications of the final product, and is preferably 30 μm or more, more preferably 50 μm or more, from the viewpoint of preventing warping. On the other hand, if the thickness is too large, the product becomes large, so the thickness is preferably 500 μm or less, more preferably 300 μm or less.
[0020] 2. Heat-adhesive resin layer The heat-adhesive resin layer of the heat-adhesive laminate of the present invention contains a polyolefin and / or an acid-modified polyolefin. The use of a polyolefin improves hydrolysis resistance, and the use of a polypropylene-based resin as the polyolefin also improves heat resistance.
[0021] Examples of polyolefins include polyethylene, polypropylene, random copolymers of propylene and ethylene, block copolymers of propylene and ethylene, random copolymers of ethylene and α-olefin, block copolymers of ethylene and α-olefin, random copolymers of propylene and α-olefin, and block copolymers of propylene and α-olefin. Examples of the α-olefins include 1-butene, isobutylene, 1-hexene, and 1-octene. Among these, polypropylene-based polymers such as polypropylene, block copolymers of propylene and ethylene, random copolymers of propylene and α-olefin, and block copolymers of propylene and α-olefin are preferred in terms of improving hot water resistance. Here, it is particularly preferred that the propylene unit content be 50% by mass or more.
[0022] Examples of acid-modified polyolefins include polymers obtained by addition or graft polymerization of an acidic group-containing monomer and / or an acid anhydride group-containing monomer to the polyolefin in the presence of a radical polymerization initiator such as an organic peroxide. Also included are polymers obtained by copolymerizing the raw material monomers of the polyolefin with an acidic group-containing monomer and / or an acid anhydride group-containing monomer. Examples of acidic group-containing monomers include acrylic acid, methacrylic acid, crotonic acid, isocrotonic acid, maleic acid, itaconic acid, and citraconic acid. Examples of acid anhydride group-containing monomers include maleic anhydride and citraconic anhydride. Among these, maleic anhydride-modified polypropylene resins (containing 50% or more propylene units by mass) are more preferred, and maleic anhydride-modified polypropylene is particularly preferred, due to their enhanced adhesion to metals and excellent hot water resistance. The acid value is preferably in the range of 0.01 to 3.0 mgKOH / g, more preferably 0.1 to 1.0 mgKOH / g.
[0023] These polyolefins may be mixed with thermoplastic elastomers other than polyolefins for the purposes of improving adhesive strength, adjusting the temperature and time during hot pressing, etc. Furthermore, additives such as antioxidants may be blended to enhance durability.
[0024] The thickness of the heat-adhesive resin layer is preferably 10 μm or more, more preferably 20 μm or more, from the viewpoint of adhesive strength and ability to conform to irregularities, and is preferably 100 μm or less, more preferably 80 μm or less, from the viewpoint of suppressing flow during hot pressing.
[0025] The melting point of the heat-adhesive resin layer is preferably 100° C. or higher, more preferably 120° C. or higher, from the viewpoint of hot water durability. Furthermore, for the purpose of shortening the time required for the hot pressing step, the melting point is preferably 200° C. or lower, more preferably 180° C. or lower. In the present invention, the melting point refers to the peak melting temperature measured using a differential scanning calorimeter (DSC) at a temperature rise rate of 10° C. / min from 25° C. to 230° C.
[0026] The heat-adhesive resin layer is preferably prepared in advance as a film for forming this layer. Preparing the film in advance facilitates adhesion with an active energy ray-curable adhesive, as described below. Furthermore, because a single film is prepared, it is easy to quickly produce a wide resin layer with excellent thickness accuracy.
[0027] 3. Active Energy Ray-Curable Adhesive The active energy ray-curable adhesive for the heat-adhesive laminate of the present invention is a composition containing a curable component and component (C): a photocationic polymerization initiator. The curable component contains the following components (A) and (B) as essential components: component (A): a compound having two or more glycidyl ether groups per molecule; component (B): a compound having an epoxy group other than component (A). The contents of components (A) and (B) are 10 to 99 wt% of component (A) and 1 to 90 wt% of component (B), based on 100 wt% of the total amount of the curable components; and the content of component (C) is 0.1 to 5 wt% per 100 parts by weight of the total amount of the curable components. In this invention, the term "curable component" refers to a compound that cures upon irradiation with active energy rays and includes components (A) and (B) as essential components. Components (A), (B), (C), and other components are described below.
[0028] 3.1 Component (A) The component (A) of the present invention is a compound having two or more glycidyl ether groups in one molecule.
[0029] Specific examples of component (A) include diglycidyl ethers of aliphatic diols such as ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, cyclohexanedimethylol diglycidyl ether, and 1,9-nonanediol diglycidyl ether; diglycidyl ethers of alicyclic diols such as tricyclodecane dimethanol diglycidyl ether and norbornane dimethanol diglycidyl ether; diglycidyl ethers of alkylene glycols such as diethylene glycol diglycidyl ether, triethylene glycol diglycidyl ether, dipropylene glycol diglycidyl ether, and tripropylene glycol diglycidyl ether; Polyglycidyl ethers of aliphatic polyols such as trimethylolpropane diglycidyl ether, trimethylolpropane triglycidyl ether, pentaerythritol polyglycidyl ether, and dipentaerythritol polyglycidyl ether; diglycidyl ethers of aromatic compounds such as hydroquinone diglycidyl ether, resorcinol diglycidyl ether, diglycidyl ether of bisphenol A (bisphenol A type epoxy resin), diglycidyl ether of bisphenol F (bisphenol F type epoxy resin), diglycidyl ether of brominated bisphenol A (brominated bisphenol A type epoxy resin), phenol novolac type epoxy resin, cresol novolac type epoxy resin, and biphenyl type epoxy resin; and diglycidyl ethers of hydrogenated aromatic compounds such as hydrogenated bisphenol A type epoxy resin and hydrogenated bisphenol F type epoxy resin.
[0030] Of these, it is preferable that the component (A) contains, as the component (a1), a diglycidyl ether of an aliphatic diol having 2 to 10 carbon atoms, because this reduces the viscosity of the adhesive composition. When the adhesive composition has a low viscosity, the thickness of the adhesive layer can be reduced, and the amount of components that leach out of the active energy ray-curable adhesive in hot water can be reduced.
[0031] Specific examples of the component (a1) include ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, and 1,9-nonanediol diglycidyl ether.
[0032] The content of component (A) is 10 to 99 wt% based on 100 wt% of the total amount of the curable components. If the content of component (A) is less than 10 wt%, the adhesive strength between the resin substrate and the heat-adhesive resin layer will decrease, and hot water immersion durability will also decrease. If the content of component (A) exceeds 99 wt%, curability will decrease. Taking into consideration both adhesive durability and curability, the blending ratio of component (A) is more preferably 10 to 80 wt%, more preferably 10 to 70 wt%, based on 100 wt% of the total amount of the curable components.
[0033] 3.2. Component (B) The component (B) of the present invention is a compound having an epoxy group other than the component (A). By including the component (B), it is possible to improve the curability with active energy rays. Preferred examples of the component (B) include the following components (b1), (b2), and (b3).
[0034] 1) Component (b1) Component (b1) is a compound having an alicyclic epoxy group but not an ester skeleton. Specific examples of component (b1) include (3,3',4,4'-diepoxy)bicyclohexyl, dicyclopentadiene dioxide, limonene dioxide, and hydrolysis condensates of 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane (e.g., silsesquioxane).
[0035] 2) Component (b2) Component (b2) is a compound having an alicyclic epoxy group and an ester skeleton. Specific examples of component (b2) include 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate and bis(3,4-epoxycyclohexylmethyl)adipate.
[0036] 3) Component (b3) Component (b3) is an epoxidized polybutadiene. Preferably, it is a compound in which the double bonds of polybutadiene have been epoxidized. Specific examples of commercially available products include NISSO-PB JP-100 and JP-200 manufactured by Nippon Soda Co., Ltd., and Epolead PB-3600 and PB-4700 manufactured by Daicel Corporation.
[0037] The content of component (B) is 1 to 90 wt %, preferably 20 to 90 wt %, and more preferably 30 to 90 wt %, based on 100 wt % of the total amount of the curable components. However, if particularly excellent adhesion durability after immersion in hot water is desired, the content of component (b2) is preferably 50 wt % or less based on 100 wt % of the total amount of the curable components.
[0038] 3.3 Component (C) Component (C) is a photocationic polymerization initiator. Component (C) is a compound that generates a strong acid when irradiated with active energy rays such as ultraviolet rays or electron beams, and this strong acid can initiate cationic polymerization of epoxy groups and the like.
[0039] As the component (C), various compounds can be used as long as they generate a strong acid upon irradiation with active energy rays, and sulfonium salt-based cationic photopolymerization initiators and iodonium salt-based cationic photopolymerization initiators are preferred.
[0040] Specific examples of sulfonium salt-based photocationic polymerization initiators include triarylsulfonium salts such as triphenylsulfonium hexafluorophosphate, triphenylsulfonium hexafluoroantimonate, triphenylsulfonium tetrakis(pentafluorophenyl)borate, and diphenyl-4-(phenylthio)phenylsulfonium hexafluorophosphate. Sulfonium salt-based photocationic polymerization initiators are commercially available, and specific examples thereof include CPI-100P, CPI-110P, CPI-100B, CPI-110B, CPI-101A, CPI-200K, CPI-210S, CPI-310B, CPI-310FG, CPI-410B, CPI-410S, VC-1S, and VC-1FG, manufactured by San-Apro Co., Ltd.
[0041] Specific examples of iodonium salt-based photocationic polymerization initiators include diaryliodonium salts such as diphenyliodonium tetrakis(pentafluorophenyl)borate, diphenyliodonium hexafluorophosphate, diphenyliodonium hexafluoroantimonate, di(4-t-butylphenyl)iodonium hexafluorophosphate, and tolylcumyliodonium tetrakis(pentafluorophenyl)borate. Iodonium salt-based photocationic polymerization initiators are commercially available, and specific examples include IK-1, 1K-1PC(80), and IK-1FG manufactured by San-Apro Co., Ltd., PI-2074 manufactured by Rhodia, and Omnicat 250 manufactured by IGM Resins.
[0042] The content of component (C) is 0.1 to 5 parts by weight per 100 parts by weight of the total amount of curable components. If the content of component (C) is less than 0.1 part by weight, the cationic curability will be insufficient. On the other hand, if the content of component (C) is more than 5 parts by weight, the amount of components eluted in hot water will increase.
[0043] 3.4. Other Components The active energy ray-curable adhesive for the heat-adhesive laminate of the present invention may contain components other than the components (A) to (C) described above, as long as the necessary properties such as adhesive performance and curability are not impaired. Examples of such components are shown below.
[0044] 1) Curable Components Other Than Components (A) and (B) The adhesive used in the present invention can contain a compound other than components (A) and (B) as a curable component. As the compound other than components (A) and (B), an oxetane compound is preferred, and it can be blended for the purpose of increasing the curing rate. When an oxetane compound is blended, the blending amount is preferably 50 wt % or less based on 100 wt % of the total curable components so as not to reduce the adhesive strength with the resin substrate. Specific examples of the oxetane compound include bis[(3-ethyloxetan-3-yl)methyl]ether, bis[(3-methyloxetan-3-yl)methyl]ether, bis[(oxetan-3-yl)methyl]ether, 1,4-bis[[(3-ethyloxetan-3-yl)methoxy]methyl]benzene, 1,4-bis[(3-ethyloxetan-3-yl)methoxy]benzene, 1,3-bis[(3-ethyloxetan-3-yl)methoxy]benzene, 1,2-bis[(3-ethyloxetan-3-yl)methoxy]benzene, 4,4'-bis[(3-ethyloxetan-3-yl)methyl]ether,
[0033] Examples thereof include 2,2'-bis[(3-ethyloxetan-3-yl)methoxy]biphenyl, 2,2'-bis[(3-ethyloxetan-3-yl)methoxy]biphenyl, 1,2-bis[(3-ethyloxetan-3-yl)methoxy]ethane, 1,2-bis[(3-ethyloxetan-3-yl)methoxy]propane, 1,6-bis[(3-ethyloxetan-3-yl)methoxy]hexane, 3-ethyl-3-(2-ethylhexyloxymethyl)oxetane, 3-ethyl-3-cyclohexyloxetane, 3-ethyl-3-phenoxymethyloxetane, and 3-ethyl-3-hydroxymethyloxetane.
[0045] 2) Photosensitizer When the active energy ray is light such as ultraviolet light, the active energy ray-curable adhesive of the heat-adhesive laminate of the present invention may contain a photosensitizer. In particular, when the photoinitiator is an iodonium salt, it is preferable to incorporate 0.1 to 2 parts by weight of the photosensitizer per 100 parts by weight of the total amount of the curable components. Specific examples of photosensitizers include anthracene-based compounds such as 9,10-dibutoxyanthracene and 9,10-diethoxyanthracene; thioxanthone-based compounds such as 2-chlorothioxanthone, 2,4-diethylthioxanthone and isopropylthioxanthone; benzophenone-based compounds such as benzophenone and 4-phenylbenzophenone; and acetophenone-based compounds such as 1-hydroxycyclohexyl phenyl ketone and 2-hydroxy-2-methyl-1-phenylpropan-1-one.
[0046] 3) Additives The active energy ray-curable adhesive of the heat-adhesive laminate of the present invention may contain additives such as antioxidants, polymerization inhibitors, leveling agents, and antifoaming agents. The content of these additives is preferably 1 part by weight or less, and more preferably 0.5 parts by weight or less, per 100 parts by weight of the total amount of the curable components. Examples of antioxidants include hindered phenol-based antioxidants, sulfur-based antioxidants, phosphorus-based antioxidants, and hindered amine-based antioxidants. Examples of polymerization inhibitors include amine-based compounds. Examples of leveling agents and antifoaming agents include silicone-based and fluorine-based compounds.
[0047] 4) Resin The active energy ray-curable adhesive of the heat-adhesive laminate of the present invention may contain a resin such as a polymer or a tackifier for the purpose of increasing adhesive strength, etc. Examples of polymers include polyethylene, polypropylene, chlorinated polypropylene, acid-modified polypropylene, polystyrene, polybutadiene, styrene-butadiene copolymer, and hydrogenated styrene-butadiene-butadiene copolymer. When these resins are contained, the amount of the resin contained is preferably 20 parts by weight or less, and more preferably 10 parts by weight or less, per 100 parts by weight of the total amount of the curable components, in order to improve coatability by suppressing an increase in viscosity, etc.
[0048] 3.5. Cured layer of active energy ray-curable adhesive In the present invention, the above-described active energy ray-curable adhesive is cured by active energy rays such as ultraviolet rays, visible light, and electron beams. The coating method and curing conditions will be explained in the manufacturing method described below. The thickness of the cured layer is preferably 1 to 10 μm, more preferably 1 to 5 μm. By making the cured layer 10 μm or less, it is possible to reduce components that dissolve in hot water. Furthermore, by making the thickness 1 μm or more, it is possible to reduce coating defects.
[0049] 4. Heat-Adhesive Laminate The heat-adhesive laminate of the present invention is a laminate comprising a resin substrate, a cured product layer of an active energy ray-curable adhesive provided on at least one surface of the resin substrate, and a heat-adhesive resin layer provided on the surface of the cured product layer opposite the resin substrate. An example of the heat-adhesive laminate of the present invention is shown in Figure 1. Figure 1 is a cross-sectional view of the heat-adhesive laminate. In Figure 1, a cured product layer (12) of an active energy ray-curable adhesive and a heat-adhesive resin layer (13) are laminated on both sides of a resin substrate (11). Another embodiment of the present invention includes a laminate in which a cured product layer (12) of an active energy ray-curable adhesive and a heat-adhesive resin layer (13) are laminated on only one side of a resin substrate (11).
[0050] 5. Manufacturing Method of Heat-Adhesive Laminate The manufacturing method of the heat-adhesive laminate of the present invention is not limited, but an example of a preferred manufacturing method and manufacturing conditions is shown below. Also described is a manufacturing method for manufacturing a heat-adhesive laminate having a hole in the shape of a picture frame or the like while suppressing the amount of waste of expensive resin substrates.
[0051] 5.1. An example of a preferred method for producing a heat-adhesive laminate In a method for producing the heat-adhesive laminate of the present invention, it is preferable to mold the resin substrate and the heat-adhesive resin layer separately as films or sheets in advance. It is also preferable to subject the adhesive surfaces to a surface treatment for easy adhesion, such as a corona discharge treatment. After this, it is preferable to apply an active energy ray-curable adhesive composition to one of the resins, and then bond them together and irradiate them with active energy rays to cure and bond them.
[0052] As the surface treatment for improving adhesion, corona discharge treatment is particularly preferred, but plasma treatment, surface roughening treatment, etching treatment, flame treatment, etc. may also be used.
[0053] Various types of coating devices for the active energy ray-curable adhesive composition can be used, including, for example, gravure coaters, microgravure coaters, die coaters, sprayers, ink jet coaters, dispensers, jet dispensers, and screen printing devices.
[0054] Examples of active energy rays include electron beams, ultraviolet rays, and visible light, with ultraviolet rays being most preferred. Examples of ultraviolet light sources include high-pressure mercury lamps, metal halide lamps, electrodeless UV lamps, and LEDs. Examples of LED wavelengths include 365 nm, 385 nm, and 405 nm. Among these, high-pressure mercury lamps, metal halide lamps, and electrodeless UV lamps are particularly preferred because they have an excellent curing speed and tend to provide excellent adhesion to resin substrates.
[0055] The amount of ultraviolet light to be applied may be appropriately determined depending on the adhesive composition and the light source. For example, when a high-pressure mercury lamp is used, the amount of ultraviolet light to be applied is 100 to 1,000 mJ / cm in the UV-B region (near 310 nm). 2 It is preferable to set the irradiation intensity to 100 mJ / cm. 2 By setting the curing amount to 1,000 mJ / cm or more, sufficient curing can be achieved. 2 The production speed can be made sufficient by the following.
[0056] When the active energy rays are ultraviolet rays, the ultraviolet rays are preferably irradiated from the heat-adhesive resin layer side, because the heat-adhesive resin layer in the present invention is mainly composed of a polyolefin-based material and has excellent ultraviolet transmittance.
[0057] After irradiation with active energy rays, the composition may be heated to an appropriate temperature. Although the heating step is not essential, heating enables curing with a small amount of irradiation, enabling high-speed production. The heating temperature at this time is preferably 60 to 130°C, more preferably 80 to 110°C. The heating time is preferably about 1 second to 2 minutes. Examples of heating methods include passing the composition through a heated atmosphere, irradiating it with infrared rays, and wrapping the composition around a heated roll.
[0058] 5.2. Preferred Manufacturing Method of Heat-Adhesive Laminate with Holes In fuel cells or water electrolysis devices, frame-shaped laminates are used. However, because the area of these holes is large, if the laminate is manufactured first and then punched out into a product, the amount of expensive resin substrate waste increases. Because the laminate of the present invention uses an active energy ray-curable adhesive, a manufacturing method that solves this problem has become possible. The manufacturing method is described below with reference to Figures 2 to 6.
[0059] 2 is a side view of the process in which holes are punched in a punching machine (22) while a rolled resin substrate sheet (21) is being fed out and then wound into a roll (25). The punched resin substrate is recovered (23) and can be reused as a raw material for producing a new resin substrate sheet. When winding into a roll, an inexpensive protective film (24) with adhesive may be attached, although this is not essential. This protective film prevents blocking of the resin substrate and maintains good flatness of the perforated resin substrate.
[0060] Figure 3 is a top view of the front and rear of the punching machine (22) (or (32) in Figure 3) in Figure 2. In Figure 3, (32) is the punching machine, and (31) is the resin substrate film. The perforated portion of (31) is the portion of the resin substrate that can be reused.
[0061] FIG. 4 is a side view of a process for producing a laminate using the resin substrate (perforated resin substrate) wound up in FIG. 2 . The side of the perforated resin substrate (41) without the protective film is subjected to corona treatment (43). A heat-sensitive adhesive resin film (42) is also subjected to corona treatment, and an adhesive is applied to this side (44). The adhesive-coated side and the corona-treated side of the resin substrate are bonded together, and the adhesive is cured using an ultraviolet irradiation device (45). In this example, the adhesive is then completely cured by passing through a heating oven (46). The protective film is then peeled off from the resin substrate and the substrate is wound up (47). Next, the newly exposed resin substrate is subjected to corona treatment (43), and a heat-sensitive adhesive resin film that has been separately corona-treated and coated with adhesive is bonded to the resin substrate. After UV curing and heating, the substrate is wound up as a semi-finished product (48).
[0062] A cross-sectional view of a portion of this semi-finished laminate (48) corresponding to one frame-shaped product is shown in Figure 5. The cured layer (52) of the active energy ray-curable adhesive and the heat-adhesive resin layer (53) cover the entire surface, but because the former is thin and the latter is made of a relatively inexpensive material, the cost of the discarded material is small even if the area to be punched out is large.
[0063] Figure 6 is a top view of the laminate (semi-finished product) shown in Figure 5, with only the resin substrate portion indicated by diagonal lines. To obtain the final product, the dotted line portion in Figure 6 is first punched out. At this time, the white blank area and the area surrounded by the dotted line represent the area of the resin substrate to be discarded. This area is much smaller than when punching out from a laminate without holes. After punching out the dotted line portion, the thick solid line portion in Figure 6 is punched out. The punched-out portion is the final product, which can be suitably used as a fuel cell or a water electrolysis device.
[0064] The above is an example of a method for producing a heat-adhesive laminate, characterized in that a hole smaller than the hole required for the final product (i.e., a hole penetrating the heat-adhesive laminate) is pre-drilled in the resin substrate, the active energy ray-curable adhesive is applied to the adhesive surface of the heat-adhesive resin film, and then the two are laminated together. The adhesive is cured and bonded by irradiating with active energy rays, and then a hole of the desired size required for the final product is drilled through the pre-drilled hole and its surrounding area. This is an example for easy understanding and is not intended to be limiting. For example, a protective film for the resin substrate, a heating furnace, etc. are not required. Corona treatment may be replaced by other treatment methods, or may be omitted if the required adhesiveness can be ensured. The ultraviolet irradiation device may be replaced by an electron beam irradiation device. The substrate and film do not need to be in roll form, but may be in sheet form. The coating method may also be replaced by spraying or screen printing.
[0065] The present invention will be explained in more detail below with reference to examples and comparative examples. However, the present invention is not limited to these examples. In the following, "parts" means parts by weight, and the numerical values showing the blending ratios in the tables mean parts by weight.
[0066] 1. Synthesis Example 1 A 3 L four-neck separable flask was charged with 962 g (0.48 mol of hydroxyl groups) of GI-3000 (hydroxyl value 28.0 mg KOH / g, Mn approximately 4,000) manufactured by Nippon Soda Co., Ltd., a hydrogenated polybutadiene having hydroxyl groups at both ends, 0.75 g of 2,6-di-t-butyl-p-cresol, and 448 g of isobornyl acrylate (hereinafter referred to as "IBXA"), and the contents were dissolved by stirring using a stirrer. A thermometer, gas inlet tube, dropping funnel, and reflux condenser were attached to the flask, and the contents were stirred while bubbling a mixed gas of oxygen and nitrogen (5% oxygen) through the flask, and the temperature was further raised to 50°C. After adding 0.03 g of ferric acetylacetonate as a catalyst and dissolving it in this solution, 66.6 g of isophorone diisocyanate (0.60 mol as isocyanate groups) was added via a dropping funnel. After stirring and mixing at 80°C for 2 hours, 17.3 g of 4-hydroxybutyl acrylate (hereinafter referred to as "HBA") (0.12 mol as hydroxyl groups) was added and the reaction was allowed to proceed for 5 hours. The disappearance of the isocyanate groups was confirmed by IR spectroscopy, and the synthesis was terminated. The resulting product was a mixture containing 70% polyurethane acrylate having a hydrogenated polybutadiene skeleton (hereinafter referred to as "PUA-1") and 30% IBXA as a diluent monomer. GPC analysis of the resulting product confirmed the peak of the PUA-1 component, distinguishable from the monomer components. The polystyrene-equivalent molecular weight of the PUA-1 component was 19,000 in Mn and 34,500 in Mw.
[0067] <Molecular Weight Measurement> Using a gel permeation chromatograph (HLC-8320 manufactured by Tosoh Corporation), Mn (number average molecular weight) and Mw (weight average molecular weight) in terms of polystyrene were obtained under the following conditions. Measurement conditions: Column: TSKgel-SuperMultipore HZ-M (4.6 mm ID x 15 cm) x 3 (for low molecular weight, exclusion limit molecular weight 2,000,000 manufactured by Tosoh Corporation) Column temperature: 40°C Eluent: tetrahydrofuran (0.35 ml / min) Detector: RI Sample concentration: 0.1%
[0068] 2. Examples 1 to 12, Comparative Examples 1 to 41) Production of active energy ray-curable adhesives 1 to 10, adhesives 1' and 2' The components shown in Table 1 below were blended in the parts by weight shown in Table 1, and stirred and mixed in a conventional manner to obtain active energy ray-curable adhesives. The parts by weight of IK-1 (PC80) in Table 1 indicate the blend amount of this product, and the number in parentheses indicates the parts by weight of component (C), which is the active ingredient. The abbreviations in Table 1 have the following meanings.
[0069] ◆ Component (A) BD-DGE: 1,4-butanediol diglycidyl ether (distilled and purified product). Epogosey BD (D) manufactured by Yokkaichi Chemical Co., Ltd. ◆ Component (B) ○ Component (b1) CEL-8000: (3,3',4,4'-diepoxy)bicyclohexyl. CELLOXIDE 8000 manufactured by Daicel Corporation. ○ Component (b2) CEL-2021: 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate. CELLOXIDE 2021P manufactured by Daicel Corporation. ○ Component (b3) JP-100: Epoxidized polybutadiene. NISSO-PB JP-100 manufactured by Nippon Soda Co., Ltd. ◆ Component (C) IK-1 (PC80): Iodonium salt-based cationic photopolymerization initiator. IK-1 (PC80) manufactured by San-Apro Co., Ltd. 80% active ingredient, 20% propylene carbonate. CPI-310B: Sulfonium salt-based photocationic polymerization initiator. CPI-310B manufactured by San-Apro Co., Ltd. Other ingredients: OXT-221: Bis[(3-ethyloxetan-3-yl)methyl]ether. Aronoxetane OXT-221 manufactured by Toagosei Co., Ltd. DBA: 9,10-dibutoxyanthracene. Anthracure UVS-1331 manufactured by Air Water Performance Chemicals Inc. Photosensitizer.
[0070]
[0071] 2) Production of active energy ray-curable adhesive 3' 40 parts of lauryl acrylate (LA) was blended and dissolved in 60 parts of the product of Synthesis Example 1, and then 1 part of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (manufactured by IGM Resins, trade name: Omnirad TPO) was added as a photoradical polymerization initiator and dissolved to produce adhesive 3'. The breakdown of this adhesive composition was 42 parts of PUA-1, 18 parts of IBXA, 40 parts of LA, and 1 part of TPO.
[0072] 3) Preparation of Substrate and Heat-Adhesive Resin Film PPSU, PESU, and PSU were used as the substrates (core materials). Radel R-5000 manufactured by Solvay was used as the PPSU, Sumikaexcel 4800P manufactured by Sumitomo Chemical Co., Ltd. was used as the PESU, and Ultrason S2010 manufactured by BASF was used as the PSU. Using these materials, a 100 μm thick film was produced using a T-die extruder. For the PEN used as the substrate for the comparative example, Teonex Q51 film (100 μm thick) manufactured by Teijin Limited was used. For the heat-adhesive resin film, a composition (acid-modified PP resin) containing 95 wt% of a mixture of maleic anhydride-modified polypropylene and polypropylene (maleic anhydride unit 0.08 wt%) and 5 wt% of a styrene-ethylene / propylene-styrene type block copolymer (styrene unit 30 wt%) was used, and a 50 μm thick film was produced using a T-die extruder.
[0073] 4) Production of a heat-adhesive laminate First, a corona discharge surface treatment device A3SW-LW manufactured by Wedge Co., Ltd. was used on both sides of the substrate and one side of the heat-adhesive resin film (using a SUS wire electrode, the distance to the stage was 10 mm), with an output of 6 W / cm and a treatment speed of 6.7 cm / sec, one round trip (treatment density 1.8 J / cm 2 ) was subjected to a corona discharge treatment. Next, one of Adhesives 1 to 10 or Adhesives 1' to 3' was applied to the corona-treated surface of the heat-sensitive adhesive resin film to a thickness of 4 μm using a bar coater, and then the substrate was laminated using a pressure roller. Next, a high-pressure mercury lamp manufactured by Eye Graphics Co., Ltd. was used, with an output of 120 W / cm, a lamp height of 15 cm, and a speed of 7 m / min (300 mW / cm for UV-B).2 , 300 mJ / cm 2 The heat adhesive resin film was irradiated with ultraviolet light from the heat adhesive resin film side to obtain a laminate. The same operation was carried out using another heat adhesive resin film and the laminate, to produce a heat adhesive laminate in which an active energy ray-curable adhesive layer and a heat adhesive resin film were laminated on both sides of the substrate.
[0074] 5) Thermocompression bonding of SUS plates using a heat-adhesive laminate A 0.1 mm thick SUS304 plate (hereinafter simply referred to as SUS plate) was cut into a size of 60 mm x 20 mm. The heat-adhesive laminate was also cut into a size of 10 mm x 55 mm. This was placed on top of the SUS plate with the long sides aligned and close to one of the long sides. Another SUS plate of the same size was placed on top of this. These were pressed at 0.55 kN (1 MPa) for 3 seconds using a pressure hot press heated to 180°C to obtain a bonded sample of SUS plates. The above procedure was repeated to obtain the required number of samples.
[0075] 6) Measurement of Adhesion Strength (T-Peel Strength) in 95°C Hot Water. Adhesion samples with a width of 10 mm were cut from the above-described SUS plate-to-SUS plate adhesion samples. The edge of the short side where the thermal adhesive laminate was not placed was cut off, resulting in one to five adhesive samples being cut out. The SUS plate on the cut-out adhesive sample where the thermal adhesive laminate was not placed was bent 90° to form a T-shape. Hooks were attached to both ends of the bent SUS plate. A water bath with hooks attached to the bottom and a tensile tester placed above the bath were prepared. 95°C water was placed in the water bath, and one hook of the adhesive sample was attached. The other hook of the adhesive was attached to the hook on the tensile tester. After immersion in 95°C water for 1 minute, the T-peel strength was measured at a tensile speed of 30 mm / min. The adhesive strength was measured at a position 2 mm from the point where the maximum adhesive strength was measured. The above measurement was performed three times, and the average value was taken as the adhesive strength. The details and results of the experiments conducted are shown in Table 2.
[0076] 7) 120°C Hot Water Immersion Test (Durability Test) The adhesive samples obtained in 5) above were immersed in a pressure-resistant container filled with pure water and held at 120°C for 1000 hours. After 1000 hours, the adhesive strength of the samples was measured in the same manner as in 6) above. The results are shown in Table 2.
[0077]
[0078] 8) Explanation of Evaluation Results In Examples 1 to 12, even after a durability test in which the samples were immersed in 120°C hot water for 1,000 hours, the adhesive strength in 95°C hot water was 2 N / cm or more. On the other hand, in Comparative Example 1, in which the substrate in Example 1 was changed from PPSU to PEN, one of the SUS sheets fell off due to the slight force applied when the sample was placed in 95°C hot water after the durability test. Observation of the location of the fracture revealed that the PEN substrate itself had become brittle and fractured. In Comparative Examples 2 and 3, in which the active energy ray-curable adhesive did not contain component (A), the adhesive strength with PPSU was weak even before the durability test, and one of the SUS sheets fell off when the sample was placed in 95°C hot water to be set. Comparative Example 4, which used a hydrophobic acrylate-based active energy ray-curable adhesive 3′, also had weak adhesive strength in 95°C hot water before the durability test. Furthermore, after the durability test, the adhesive strength had decreased to the point where one of the SUS sheets fell off when the sample was placed in the hot water. Comparing Examples 1 to 12, Examples 6 and 7, in which the active energy ray-curable adhesive contained 50 parts by weight or more of a compound having an alicyclic epoxy group and an ester skeleton (component (b2)) based on 100 parts by weight of the total curable components, showed a relatively large decrease in adhesive strength after the durability test. Furthermore, Example 3, which used Adhesive 3 containing 75 parts of component (A), showed slightly lower adhesive strength than Examples 1 and 2 before and after the durability test. Examples 1 and 8 to 12, which used Adhesive 1, Adhesive 8, Adhesive 9, and Adhesive 10, showed fracture in the T-peel test at the SUS interface, and the laminates remained strong, even after a durability test in which they were immersed in hot water at 120°C for 1,000 hours. As shown in Examples 11 and 12, it was confirmed that not only PPSU but also PESU and PSU exhibited excellent durability.
[0079] 3. Comparative Example 51) Production of heat-adhesive laminate Preparation of easy adhesive An easy adhesive (solid content concentration 4% by weight) was prepared according to the following recipe. Ion-exchanged water was used as the dilution solvent. Acrylic resin (manufactured by Nippon Carbide Industries Co., Ltd., trade name RX7770): 85 parts by weight Epoxy-based crosslinking agent (manufactured by Mitsubishi Gas Chemical Company, Inc., trade name TETRAD-X): 7.5 parts by weight Surfactant (manufactured by Sanyo Chemical Industries, Ltd., trade name Sannonic SS-70): 7.5 parts by weight
[0080] ○ Production of Resin Substrate Having Easy-Adhesion Layer Polyethylene-2,6-naphthalate (PEN) with an intrinsic viscosity of 0.60 dl / g (35°C, orthochlorophenol) was synthesized using manganese acetate tetrahydrate as a transesterification catalyst and antimony trioxide as a polymerization catalyst. The resulting resin was dried in a 170°C dryer for 6 hours, then fed into an extruder and melt-kneaded at a melt temperature of 300°C. The resin was extruded through a die slit at 300°C and cooled and solidified on a casting drum set at a surface temperature of 25°C to produce an unstretched film. This unstretched film was introduced into a group of rolls heated to 140°C, stretched 3.5 times in the longitudinal direction, and cooled with a group of rolls at 25°C. The above-mentioned easy-adhesive was applied to both sides of the longitudinally stretched film using a roll coater method so that the thickness of the easy-adhesion layer in the final laminate was 50 nm. Subsequently, the film was introduced into a tenter while holding both ends with clips, and stretched 3.5 times in the transverse direction in an atmosphere heated to 135° C. In the tenter, the film was heat-set at 220° C. for 40 seconds, relaxed 1% in the transverse direction at 220° C., and then uniformly cooled slowly to room temperature to obtain a biaxially stretched film having a thickness of 200 μm.
[0081] Formation of heat-adhesive resin layer Next, the above-mentioned acid-modified PP-based resin layer was formed on the adhesive layer on both sides of the obtained biaxially stretched film by extrusion lamination (230 ° C), to obtain a heat-adhesive laminate. Each of the obtained heat-adhesive resin layers had a thickness of 50 μm.
[0082] 2) Evaluation of heat-adhesive laminate The obtained laminate was subjected to adhesion between SUS plates, measurement of adhesive strength in 95°C hot water, and a 120°C hot water immersion test in the same manner as in Example 1, and the results are shown in Table 2. As a result, the adhesive strength in 95°C hot water was excellent before the durability test, but after immersion in 120°C hot water for 1000 hours, it had dropped significantly to 0.5 N / cm. Observation of the fracture site revealed that the PEN substrate itself had become brittle and fractured.
[0083] The heat-adhesive laminate of the present invention can be suitably used as a material for thermocompression bonding of metal members and the like in places where heat resistance and hydrolysis resistance are required, and is particularly suitable as a member for fuel cells and water electrolysis devices.
[0084] DESCRIPTION OF SYMBOLS 11: Resin substrate 12: Cured layer of active energy ray-curable adhesive 13: Heat-adhesive resin layer 21: Roll of resin substrate film 22: Punching machine 23: Resin substrate collection box 24: Roll of protective film 25: Roll of punched substrate film 31: Resin substrate film 32: Punching machine 41: Roll of resin substrate film 42: Roll of heat-adhesive resin film 43: Corona discharge treatment machine 44: Active energy ray-curable adhesive and applicator 45: Ultraviolet irradiator 46: Heating furnace 47: Protective film take-up roll 48: Laminate (semi-finished product) take-up roll 51: Resin substrate 52: Cured layer of active energy ray-curable adhesive 53: Heat-adhesive resin layer
[0085] The disclosure of Japanese Patent Application No. 2023-049649, filed on March 27, 2023, is incorporated herein by reference in its entirety. All publications, patent applications, and technical standards mentioned herein are incorporated herein by reference to the same extent as if each individual publication, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.
Claims
1. A laminate comprising a resin substrate, a cured product layer of an active energy ray curable adhesive provided on at least one surface of the resin substrate, and a heat-adhesive resin layer provided on a surface of the cured product layer opposite to the resin substrate, wherein the resin substrate comprises at least one selected from the group consisting of polyphenylsulfone, polyethersulfone, and polysulfone, the heat-adhesive resin layer comprises a polyolefin and / or an acid-modified polyolefin, and the active energy ray curable adhesive is a composition containing a curable component and component (C): a photocationic polymerization initiator, the curable component comprising the following components (A) and (B) as essential components, component (A): a compound having two or more glycidyl ether groups in one molecule, component (B): a compound having an epoxy group other than component (A), the content ratios of components (A) and (B) are 10 to 99% by weight for component (A) and 1 to 90% by weight for component (B), relative to 100% by weight of the total amount of the curable components, The content of the component (C) is 0.1 to 5 parts by weight per 100 parts by weight of the total amount of the curable components.
2. The heat-adhesive laminate according to claim 1, wherein component (A) contains (a1) a diglycidyl ether of an aliphatic diol having 2 to 10 carbon atoms.
3. The heat-adhesive laminate according to claim 2, wherein the component (B) contains at least one compound selected from the group consisting of (b1) a compound having an alicyclic epoxy group and no ester skeleton, (b2) a compound having an alicyclic epoxy group and an ester skeleton, and (b3) an epoxidized polybutadiene.
4. The heat-adhesive laminate according to claim 3, wherein the active energy ray-curable adhesive does not contain 50% by weight or more of component (b2) out of a total of 100% by weight of the curable components.
5. The heat-adhesive laminate according to claim 1, further comprising an oxetane compound as a curable component in the active energy ray-curable adhesive.
6. The heat-adhesive laminate according to claim 1, which is used as a component of a polymer electrolyte fuel cell or a water electrolysis device.
7. A method for producing a heat-adhesive laminate as described in claim 1, comprising the steps of: (1) subjecting the adhesive surface of the resin substrate and the adhesive surface of a resin film for forming the heat-adhesive resin layer to a corona discharge treatment; and (2) bonding the resin substrate and the resin film together with an active energy ray-curable adhesive.
8. The method for producing a heat-adhesive laminate according to claim 7, further comprising the steps of: (3) drilling a hole in the resin substrate prior to step (1); and (4) drilling a hole through the heat laminate in the hole and in the surrounding area after step (2).
Citation Information
Patent Citations
Fuel battery cell and method of manufacturing fuel battery cell
JP2017103126A
Fuel battery cell
JP2019102370A
Fuel cell
JP2020198199A
laminate
JP2021054880A
Device introduction device and device introduction method
JP2023049649A
Cited By
Adhesive sheet
WO2026164246A1