Thermosetting adhesive sheet, laminate, and method for producing laminate
The thermosetting adhesive sheet, composed of specific components and manufactured into a laminate, addresses the need for low dielectric properties and bending resistance in high frequency bands, enhancing signal transmission and structural integrity in electronic devices.
Patent Information
- Application Number
- PCT/JP2024/011657
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-03
AI Technical Summary
Current adhesive sheets used in electronic devices lack both low dielectric properties and bending resistance, especially in high frequency bands, and existing resin compositions do not adequately address these requirements.
A thermosetting adhesive sheet with a specific composition including a binder resin, thermosetting component, and filler, which has a low dielectric loss tangent and high gel fraction, along with a manufacturing method to form a laminate with a conductive layer, ensuring excellent low dielectric properties and bending resistance.
The thermosetting adhesive sheet achieves low dielectric loss and high bending resistance, reducing signal transmission loss and maintaining structural integrity in high frequency bands, while the manufacturing method efficiently produces laminates with these properties.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Thermosetting adhesive sheet, laminate, and method for manufacturing laminate
[0001] The present invention relates to a thermosetting adhesive sheet having excellent low dielectric properties and flex resistance in the high frequency band, a laminate including a conductive layer and an adhesive layer of the thermosetting adhesive sheet, and a method for manufacturing the laminate.
[0002] In recent years, electronic devices have become smaller, lighter, and more powerful, and thus flexible printed circuits (FPCs) and other wiring components are being required to have higher density packaging, lighter weight, and higher reliability. Furthermore, as the speed of transmission signals in wiring components such as FPCs increases, the frequency of transmission signals is also increasing. Therefore, materials used in wiring components are being required to reduce electrical signal loss in high-frequency bands. Furthermore, adhesive sheets used in interlayer adhesive layers of wiring components and adhesive sheets used as surface protective films (i.e., coverlay films) for wiring components are also being required to have excellent low dielectric properties in high-frequency bands.
[0003] Therefore, in order to transmit high-frequency electrical signals at high speed and with reduced transmission loss, attempts have been made to improve the low dielectric properties (lower dielectric constant and lower dielectric loss tangent) of insulators (substrates, adhesives, etc.) that make up wiring members (Patent Documents 1 to 5, etc.). In addition, in recent years, electronic devices have been made lighter, thinner, shorter, and smaller, and as a result, adhesive sheets that not only have excellent electrical properties (low dielectric constant and low dielectric loss tangent) in the high-frequency band but also have excellent flex resistance have been demanded.
[0004] WO2016 / 147984 JP 2016-089137 A WO2019 / 230531 A WO2019 / 026927 A JP 2019-172803 A
[0005] However, although Patent Documents 1 to 5 above describe resin compositions having low dielectric properties, they do not describe that the resin compositions have excellent flex resistance, and the flex resistance is not satisfactory.
[0006] The present invention has been made in consideration of the above-mentioned circumstances, and aims to provide a thermosetting adhesive sheet that has excellent low dielectric properties in the high frequency band and also excellent flex resistance, a laminate having a conductive layer and an adhesive layer formed from the thermosetting adhesive sheet, and a method for manufacturing the laminate.
[0007] In order to solve the above problems, the present inventors have conducted extensive research into thermosetting adhesive sheets having an adhesive layer, and as a result have completed the present invention.
[0008] Thus, according to the present invention, there are provided the following thermosetting adhesive sheets described in [1] to [8], the laminate described in [9], and the methods for producing the laminates described in
[10] and
[11] .
[0009] [1] A thermosetting adhesive sheet having an adhesive layer, wherein the adhesive layer is a layer containing the following components (A), (B), and (C): the arithmetic mean surface roughness (Ra) of the adhesive layer surface is 200 nm or less, the dielectric loss tangent at 23°C and a frequency of 10 to 40 GHz of a cured material layer obtained by heat-treating the adhesive layer at 170°C for 2 hours is 0.005 or less, and the gel fraction of the cured material layer obtained by heat-treating the adhesive layer at 170°C for 2 hours is 40% or more. Component (A): binder resin, component (B): thermosetting component, and component (C): filler.
[0010] [2] The thermosetting adhesive sheet according to [1], wherein the gel fraction of the adhesive layer before curing is α (%) and the gel fraction of the cured material layer obtained by curing the adhesive layer is β (%), the rate of increase (%) of the gel fraction, expressed by the formula: [(β-α) / α]×100, is 60% or more.
[0011] [3] The thermosetting adhesive sheet according to [1] or [2], wherein the cured layer obtained by heat-treating the adhesive layer at 170°C for 2 hours has a tensile modulus at 25°C of 0.5 GPa or more.
[0012] [4] The thermosetting adhesive sheet according to [1] or [2], which satisfies the formula: Y / X<1, where X (μm) is the thickness of the adhesive layer and Y (μm) is the average particle size of the component (C).
[0013] [5] The thermosetting adhesive sheet according to [1] or [2], wherein the component (C) is an inorganic filler that has not been surface-treated.
[0014] [6] The thermosetting adhesive sheet according to [1] or [2], wherein the component (C) is a spherical filler.
[0015] [7] The thermosetting adhesive sheet according to [1] or [2], wherein the adhesive layer further contains a thermal polymerization initiator as component (D).
[0016] [8] The thermosetting adhesive sheet according to [1] or [2], which is used for forming an insulating layer of a device.
[0017] [9] A laminate comprising a conductive layer and an insulating layer formed on the conductive layer, wherein the insulating layer is a layer formed by curing the adhesive layer of the thermosetting adhesive sheet according to [1] or [2].
[0018]
[10] A method for producing the laminate according to [9], comprising: a step (I) of obtaining a laminate by laminating the thermosetting adhesive sheet according to [1] or [2] onto a conductive layer; and a step (II) of heating the laminate to a predetermined temperature to cure the adhesive layer of the thermosetting adhesive sheet.
[0019]
[11] The method for producing a laminate according to
[10] , comprising, after the step (I) and before the step (II), a step (I-1) of forming a protective layer on the thermosetting adhesive sheet according to [1] or [2].
[0020] According to the present invention, there is provided a thermosetting adhesive sheet having an adhesive layer that provides a cured product with excellent low dielectric properties in the high frequency band and also has excellent flex resistance. The laminate of the present invention has a layer (hereinafter sometimes referred to as the "cured product layer") formed by curing the adhesive layer of the thermosetting adhesive sheet of the present invention, and therefore has excellent low dielectric properties in the high frequency band and also has excellent flex resistance. Furthermore, according to the manufacturing method of the present invention, the laminate of the present invention can be efficiently manufactured.
[0021] 1 is a process diagram illustrating a method for producing a laminate of the present invention.
[0022] The present invention will be described in detail below, divided into the following sections: 1) a thermosetting adhesive sheet, 2) a laminate, and 3) a method for producing a laminate.
[0023] As used herein, "high frequency band" refers to the frequency range of 10 to 40 GHz. As used herein, "excellent low dielectric properties" means that the cured product layer obtained by heat-treating the adhesive layer at 170°C for 2 hours has a low dielectric dissipation factor (preferably a dielectric dissipation factor of 0.005 or less at 23°C and a frequency of 10 to 40 GHz) and exhibits low transmission loss in the high frequency band. As used herein, "excellent flex resistance" means that the thermosetting adhesive sheet has the ability to conform to deformation without being damaged. Whether or not a thermosetting adhesive sheet has excellent flex resistance can be confirmed, for example, by the flex test described in the Examples. As used herein, "relative humidity α%" may also be expressed as "α% RH" (RH; Relative Humidity).
[0024] 1) Thermosetting Adhesive Sheet The first aspect of the present invention is a thermosetting adhesive sheet having an adhesive layer, wherein the adhesive layer is (α) a layer containing the components (A), (B), and (C), (β) the arithmetic mean surface roughness (Ra) of the adhesive layer surface is 200 nm or less, (γ) the cured material layer obtained by heat-treating the adhesive layer at 170°C for 2 hours has a dielectric loss tangent of 0.005 or less at 23°C and a frequency of 10 to 40 GHz, and (δ) the cured material layer obtained by heat-treating the adhesive layer at 170°C for 2 hours has a gel fraction of 40% or more. Note that in this specification, the term "thermosetting adhesive sheet" may also be simply referred to as "adhesive sheet."
[0025] [Component (A): Binder Resin] The adhesive layer according to the present invention preferably contains a binder resin as component (A). The binder resin is a polymer component that imparts film-forming properties for forming the adhesive layer and also imparts suitable flexibility to the resulting adhesive layer. By containing a binder resin, the adhesive layer according to the present invention is more likely to retain its shape as an adhesive layer.
[0026] The binder resin is not particularly limited as long as it is a polymer component that exhibits the above-mentioned film-forming properties and imparts flexibility to the resulting adhesive layer. Examples include olefin-based resins, acrylic polymers, polyester resins, polyvinyl alcohol resins, polyvinyl butyral, polyvinyl chloride, phenoxy resins, polyamide resins, cellulose-based materials, polyvinyl ethers, polyimide resins, and styrene-based elastomers. Among these, olefin-based resins and styrene-based elastomers are preferred because they are more likely to produce cured products with excellent low dielectric properties. The binder resins can be used alone or in combination of two or more.
[0027] The olefin resin refers to a polymer containing repeating units derived from an olefin monomer. The olefin resin may be a polymer consisting only of repeating units derived from an olefin monomer, or may be a polymer consisting of repeating units derived from an olefin monomer and repeating units derived from a monomer copolymerizable with the olefin monomer. However, from the viewpoint of easily obtaining a cured product having excellent low dielectric properties, a polymer consisting only of repeating units derived from an olefin monomer is preferred.
[0028] As the olefin-based monomer, an α-olefin having 2 to 8 carbon atoms is preferred, with ethylene, propylene, 1-butene, isobutylene, or 1-hexene being more preferred, and ethylene or propylene being even more preferred. These olefin-based monomers can be used alone or in combination of two or more. Examples of monomers copolymerizable with the olefin-based monomer include vinyl acetate, (meth)acrylic acid esters, and styrene. Herein, "(meth)acrylic acid" means acrylic acid or methacrylic acid. These monomers copolymerizable with the olefin-based monomer can be used alone or in combination of two or more.
[0029] Preferred examples of the olefin resin include very low density polyethylene (VLDPE), low density polyethylene (LDPE), medium density polyethylene (MDPE), high density polyethylene (HDPE), linear low density polyethylene, polypropylene (PP), ethylene-propylene copolymer, olefin elastomer (TPO), ethylene-vinyl acetate copolymer (EVA), ethylene-(meth)acrylic acid copolymer, and ethylene-(meth)acrylic acid ester copolymer.
[0030] Examples of styrene-based elastomers include block copolymers having hard segments composed of blocks obtained by polymerization of styrene and soft segments composed of blocks obtained by polymerization of aliphatic olefins such as ethylene, butadiene, and isoprene, and hydrogenated products thereof.
[0031] Preferred specific examples of the styrene-based elastomer include styrene-butadiene copolymer, styrene-isoprene copolymer, styrene-butadiene-styrene copolymer (SBS), styrene-isoprene-styrene copolymer (SIS), styrene-isoprene-butadiene-styrene copolymer (SIBS), styrene-ethylene copolymer, styrene-ethylene-propylene-styrene copolymer (SEPS), and styrene-ethylene-butylene-styrene copolymer (SEBS).
[0032] The binder resin is preferably a resin having a reactive functional group. By using a resin having a reactive functional group as the binder resin, a crosslinked structure that easily exhibits the effects of the present invention can be constructed in the adhesive layer (and the cured product layer). In particular, it is easy to form a cured product layer that has a high gel fraction and excellent flex resistance. Furthermore, it is possible to form a cured product layer that easily adheres sufficiently to poorly adhesive substrates, etc.
[0033] Examples of the reactive functional group include a carboxyl group, a carboxylic anhydride group, a carboxylic ester group, a hydroxyl group, an epoxy group, an amide group, an ammonium group, a nitrile group, an amino group, an imide group, an isocyanate group, an acetyl group, a thiol group, an ether group, a thioether group, a sulfone group, a phosphone group, a nitro group, a urethane group, an alkoxysilyl group, a silanol group, and a halogen atom.
[0034] Examples of resins having reactive functional groups include modified polyolefin resins, which will be described later, and the above-mentioned binder resins, such as phenoxy resins and cellulose-based materials. Also, examples of the above-mentioned binder resins include modified resins other than olefin-based resins. As the binder resin, modified polyolefin resins or modified styrene-based elastomers are preferred because they have a high gel fraction and are likely to produce a cured layer that has low dielectric properties and excellent flex resistance.
[0035] Modified polyolefin resins are olefin resins into which reactive functional groups have been introduced, obtained by subjecting a precursor olefin resin to a modification treatment using a modifier (a compound having functional groups in the molecule).
[0036] The modified polyolefin resin is preferably an acid-modified polyolefin resin, since it forms a cured layer having superior adhesive strength. By curing an adhesive composition containing an acid-modified polyolefin resin, a cured layer having superior adhesive strength can be formed.
[0037] The acid-modified polyolefin resin refers to an olefin resin graft-modified with an acid or an acid anhydride, such as an olefin resin that has been reacted with an unsaturated carboxylic acid or an unsaturated carboxylic acid anhydride (hereinafter sometimes referred to as "unsaturated carboxylic acid, etc.") to introduce a carboxyl group or a carboxylic acid anhydride group (graft-modified).
[0038] Examples of unsaturated carboxylic acids to be reacted with olefin resins include unsaturated carboxylic acids such as maleic acid, fumaric acid, itaconic acid, citraconic acid, glutaconic acid, tetrahydrophthalic acid, and aconitic acid; and unsaturated carboxylic acid anhydrides such as maleic anhydride, itaconic anhydride, glutaconic anhydride, citraconic anhydride, aconitic anhydride, norbornene dicarboxylic anhydride, and tetrahydrophthalic anhydride. These can be used alone or in combination of two or more. Among these, unsaturated carboxylic acid anhydrides are preferred, and maleic anhydride is particularly preferred, as they are more likely to produce cured products with excellent adhesive strength.
[0039] The amount of the unsaturated carboxylic acid or the like reacted with the olefin resin is preferably 0.1 to 5 parts by mass, more preferably 0.2 to 3 parts by mass, and even more preferably 0.2 to 1 part by mass, per 100 parts by mass of the olefin resin.
[0040] The method for introducing the unsaturated carboxylic acid or the like into the olefin resin is not particularly limited. For example, there may be mentioned a method in which the olefin resin and the unsaturated carboxylic acid or the like are reacted by heating and melting them at a temperature equal to or higher than the melting point of the olefin resin in the presence of a radical generator such as an organic peroxide or an azonitrile, or a method in which the olefin resin and the unsaturated carboxylic acid or the like are dissolved in an organic solvent, and then heated and stirred in the presence of a radical generator to react them, thereby graft-copolymerizing the unsaturated carboxylic acid or the like onto the olefin resin.
[0041] As the acid-modified polyolefin resin, commercially available products can also be used, such as Admer (registered trademark, manufactured by Mitsui Chemicals, Inc.), Unistall (registered trademark, manufactured by Mitsui Chemicals, Inc.), BondyRam (registered trademark, manufactured by Polyram Corporation), orevac (registered trademark, manufactured by ARKEMA), and Modic (registered trademark, manufactured by Mitsubishi Chemical Corporation).
[0042] The modified styrene-based elastomer may be a styrene-based elastomer modified with an unsaturated carboxylic acid, etc. Examples of methods for modifying the styrene-based elastomer include the above-mentioned method of subjecting the styrene-based elastomer to a graft reaction with an unsaturated carboxylic acid, etc.
[0043] As the unsaturated carboxylic acid, the same unsaturated carboxylic acids as those exemplified above as the unsaturated carboxylic acids to be reacted with the olefin resin can be used.
[0044] Commercially available modified styrene elastomers include, for example, the Tuftec M series manufactured by Asahi Kasei Corporation and the Kraton FG series manufactured by Kraton Polymer Japan.
[0045] The number average molecular weight (Mn) of the binder resin is not particularly limited, but is preferably 10,000 to 150,000, more preferably 30,000 to 100,000. This not only imparts the desired film-forming properties, but also makes it easier to impart flexibility to the resulting adhesive layer, which in turn makes it easier to exhibit excellent flex resistance. The number average molecular weight (Mn) of the binder resin can be determined as a standard polystyrene equivalent value by performing gel permeation chromatography (GPC) using tetrahydrofuran (THF) as a solvent.
[0046] The content of the binder resin in the adhesive layer according to the present invention is preferably 5 to 50% by mass, more preferably 10 to 40% by mass, particularly preferably 12 to 30% by mass, and even more preferably 14 to 20% by mass. This not only provides film-forming properties for forming the adhesive layer, but also imparts suitable flexibility to the resulting adhesive layer. This makes it easier to blend materials such as the thermosetting component and crosslinking agent described below in the desired ratio. Furthermore, it also makes it easier to obtain an adhesive layer that satisfies the physical properties described below, thereby achieving both excellent low dielectric properties and flex resistance.
[0047] [Component (B): Thermosetting Component] The adhesive layer according to the present invention preferably contains a thermosetting component (hereinafter sometimes referred to as "thermosetting component (B)") as component (B). The thermosetting component (B) is a compound that has the property of undergoing a curing reaction when heated. When the above-mentioned component (A) is a resin having a reactive functional group, it also reacts with the reactive functional group to form a crosslinked structure, and can provide a cured product having the desired crosslink density.
[0048] The thermosetting component (B) is not particularly limited as long as it is a compound that undergoes a curing reaction when heated, but from the viewpoint of facilitating the formation of an adhesive layer with superior low dielectric properties and excellent flex resistance, the following components (B1) and (B2) are preferred examples. Note that component (B1) does not include component (B2). Component (B1): A thermosetting compound that is liquid at 25°C Component (B2): A polyphenylene ether resin
[0049] The thermosetting component (B) can be used alone or in combination of two or more types. In the present invention, however, from the viewpoint of facilitating the formation of an adhesive layer that combines excellent low dielectric properties and flex resistance, it is preferred to use one or more types of (B1) component in combination with one or more types of (B2) component.
[0050] The component (B1) is preferably a thermosetting compound that is liquid at 25°C (hereinafter, may be referred to as "thermosetting compound (B1)"), and is particularly preferably a non-aromatic thermosetting compound that is liquid at 25°C. Here, "liquid at 25°C" means that the compound has fluidity at 25°C. For example, a compound that is liquid at 25°C is a compound that has a viscosity of 2 to 10,000 mPa s when measured at 25°C and 1.0 rpm using an E-type viscometer.
[0051] The thermosetting compound (B1) may be any of aromatic, anti-aromatic, and non-aromatic compounds, but is preferably a non-aromatic compound from the viewpoint that the resulting adhesive layer is more likely to satisfy the physical properties described below and to achieve both low dielectric properties and flex resistance. A non-aromatic compound means a compound that does not have an aromatic ring.
[0052] The thermosetting compound (B1) preferably has a heterocyclic skeleton. This facilitates the formation of an adhesive layer that provides a cured product with superior adhesive strength and low dielectric properties. Examples of heterocyclic skeletons include an isocyanurate skeleton and a glycoluril skeleton. The heterocyclic skeleton preferably has an n-fold rotation axis as a symmetry element. An adhesive layer containing a thermosetting compound (B1) having such a heterocyclic skeleton tends to have superior low dielectric properties.
[0053] The molecular weight of the thermosetting compound (B1) is preferably 100 to 1,000, more preferably 150 to 800, even more preferably 200 to 600, and particularly preferably 250 to 500. This tends to satisfy the above-mentioned requirement of being liquid at 25°C, contributing to excellent kneadability with other materials and resulting in good film-forming properties. Furthermore, since it is less likely to volatilize even when heat treatment is performed during the formation or use of the adhesive layer, it is easier to obtain a cured product having the physical properties described below. In particular, the resulting cured product layer is more likely to exhibit good flex resistance.
[0054] A preferred example of the thermosetting compound (B1) is a compound having two or more hydrocarbon groups each having a double bond at its terminal (hereinafter, this compound may be referred to as a "thermosetting compound (B1')"). Use of the thermosetting compound (B1') makes it easier to form an adhesive layer that gives a cured product with excellent low dielectric properties.
[0055] The number of carbon atoms in the hydrocarbon group having a terminal double bond is preferably 1 to 10, more preferably 2 to 5, and particularly preferably 3 to 4. Examples of the hydrocarbon group having a terminal double bond include vinyl, allyl, 3-butenyl, 4-pentenyl, 5-hexenyl, isopropenyl, 1-methyl-2-propenyl, vinylbenzyl, and vinylnaphthyl groups. Among these, vinyl and allyl groups are preferred, with allyl groups being particularly preferred. The number of hydrocarbon groups having a terminal double bond is preferably 1 or more, and particularly preferably 2 or more. This facilitates the formation of an adhesive layer that satisfies the physical properties described below and provides a cured product with superior adhesive strength and heat resistance. In particular, the resulting cured product layer is more likely to exhibit good flex resistance. The upper limit of the number of hydrocarbon groups is not limited, but is preferably 10 or less, more preferably 6 or less, even more preferably 4 or less, and particularly preferably 3 or less, from the viewpoint of suppressing cracking by appropriately sparsely distributing the crosslinked structure formed in the cured product.
[0056] Examples of the thermosetting compound (B1') include a thermosetting compound having an isocyanurate skeleton and a thermosetting compound having a glycoluril skeleton. Examples of the thermosetting compound having an isocyanurate skeleton include compounds represented by the following formula (1) or (2):
[0057]
[0058] In formula (1), R 1 , R 2 each independently represents a hydrocarbon group having a double bond at its terminal, R 3 represents a saturated hydrocarbon group having 1 to 15 carbon atoms or an alkoxy-substituted alkyl group having 2 to 15 carbon atoms.
[0059]
[0060] In formula (2), R 4 , R 5 , R 6 each independently represents a hydrocarbon group having a double bond at its terminal.
[0061] R 1 , R 2 , R 4 , R 5 , R 6 The hydrocarbon group having a double bond at the terminal, represented by the formula: is as described above.
[0062] R 3 The saturated hydrocarbon group represented by the formula (I) preferably has 1 to 15 carbon atoms, more preferably 5 to 15 carbon atoms, and even more preferably 8 to 15 carbon atoms. 3 Preferred examples of the saturated hydrocarbon group represented by the formula (I) include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a t-butyl group, an s-butyl group, an isobutyl group, an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, an n-decyl group, an n-undecyl group, an n-dodecyl group, an n-tridecyl group, an n-tetradecyl group, and an n-pentadecyl group.
[0063] R 3 The number of carbon atoms in the alkoxy-substituted alkyl group represented by R is 1 to 15, preferably 2 to 12, and more preferably 3 to 10.3 Preferred examples of the alkoxy-substituted alkyl group represented by the formula (I) include a methoxymethyl group, an ethoxymethyl group, a 2-methoxyethoxymethyl group, and a benzyloxymethyl group.
[0064] Examples of the thermosetting compound having a glycoluril skeleton include compounds represented by the following formula (3).
[0065]
[0066] In formula (3), R 7 , R 8 , R 9 , R 10 are each independently a hydrocarbon group having 1 to 15 carbon atoms, and at least two of these are hydrocarbon groups having a double bond at the terminal. 11 , R 12 is a hydrogen atom or a saturated hydrocarbon group having 1 to 15 carbon atoms.
[0067] Among these, as the thermosetting compound (B1′), a compound having an isocyanurate skeleton is preferred, a compound represented by formula (1) is more preferred, and a compound represented by the following formula is even more preferred, because it is easy to obtain a cured product that satisfies the physical properties described below, has an appropriate crosslinking density, and is excellent in low dielectric properties and flex resistance.
[0068]
[0069] In the formula, R represents a saturated hydrocarbon group having 5 to 15 carbon atoms, and preferably a saturated hydrocarbon group having 8 to 15 carbon atoms.
[0070] When the adhesive layer contains the thermosetting compound (B1), the content thereof in the adhesive layer is preferably 5 to 50 mass %, more preferably 10 to 40 mass %, even more preferably 15 to 30 mass %, and particularly preferably 18 to 25 mass %. This makes it easier to form an adhesive layer that satisfies the physical properties described below and provides a cured product layer that is excellent in adhesive strength and low dielectric properties. In particular, the resulting cured product layer is more likely to exhibit good flex resistance.
[0071] The component (B2) is a polyphenylene ether resin (hereinafter, sometimes referred to as "polyphenylene ether resin (B2)"). The polyphenylene ether resin refers to a resin having a polyphenylene ether skeleton in the main chain. The polyphenylene ether skeleton refers to a skeleton having a repeating unit represented by the following formula or a repeating unit obtained by substituting a hydrogen atom in the above formula:
[0072]
[0073] Since the polyphenylene ether resin (B2) has a polyphenylene ether skeleton, an adhesive layer containing the polyphenylene ether resin (B2) has excellent low dielectric properties. Furthermore, the polyphenylene ether resin (B2) preferably has a reactive functional group. This makes it easier for the cured product of the adhesive layer to satisfy the physical properties described below and to have excellent heat resistance and flex resistance.
[0074] The polyphenylene ether skeleton may be one represented by the following formula (4).
[0075]
[0076] In formula (4), X is a divalent group represented by the following formula (5) or formula (6), and each Y is independently a divalent group represented by the following formula (7). a and b are integers from 0 to 100, and at least one of a and b is 1 or greater. * represents a bond (the same applies hereinafter).
[0077]
[0078] In formula (5), R 13 , R 14 , R 15 , R 16 , R 17 , R 18 , R 19 , R 20 are each independently a hydrogen atom, a halogen atom, an alkyl group having 6 or less carbon atoms, or a phenyl group, and are preferably a hydrogen atom or a methyl group.
[0079]
[0080] In formula (6), R21 , R 22 , R 23 , R 24 , R 25 , R 26 , R 27 , R 28 are each independently a hydrogen atom, a halogen atom, an alkyl group having 6 or less carbon atoms, or a phenyl group, and are preferably a hydrogen atom or a methyl group. A is a linear, branched, or cyclic divalent hydrocarbon group having 20 or less carbon atoms.
[0081]
[0082] In formula (7), R 29 , R 30 , R 31 , R 32 are each independently a hydrogen atom, a halogen atom, an alkyl group having 6 or less carbon atoms, or a phenyl group, and are preferably a hydrogen atom or a methyl group.
[0083] Specific examples of the polyphenylene ether skeleton include those represented by the following formulas (8a) and (8b), but are not limited thereto.
[0084]
[0085]
[0086] In formulas (8a) and (8b), a and b are integers of 0 to 100, and at least one of a and b is 1 or greater.
[0087] Examples of the reactive functional group in the polyphenylene ether resin (B2) include groups having an ethylenically unsaturated bond, such as a vinyl group, an allyl group, an acryloyl group, a methacryloyl group, a cyclopentenyl group, a vinylbenzyl group, and a vinylnaphthyl group; an epoxy group; a hydroxyl group; etc. Among these, a group having an ethylenically unsaturated bond is preferred because it is easy to satisfy the physical properties described below and to obtain a cured product having excellent low dielectric properties, and from the viewpoint of easily obtaining a cured product that easily exhibits flex resistance, a methacryloyl group or a vinylbenzyl group is more preferred, and a vinylbenzyl group is even more preferred.
[0088] The polyphenylene ether resin (B2) having a reactive functional group is preferably one having a reactive functional group at any position of the polyphenylene ether skeleton, and more preferably one having a reactive functional group at both ends of the polyphenylene ether skeleton, which makes it easier to obtain a cured product that satisfies the physical properties described below and has excellent low dielectric properties and flex resistance.
[0089] The number average molecular weight (Mn) of the polyphenylene ether resin (B2) is not particularly limited, but is preferably 500 to 5,000, more preferably 500 to 3,000. This makes it easier to obtain a cured product that satisfies the physical properties described below and has excellent low dielectric properties and flex resistance. It also makes it easier to achieve excellent adhesion to the adherend. The number average molecular weight (Mn) can be determined as a standard polystyrene equivalent value by gel permeation chromatography (GPC) using tetrahydrofuran (THF) as a solvent.
[0090] When the adhesive layer contains a polyphenylene ether resin (B2), its content in the adhesive layer is preferably 10 to 70% by mass, more preferably 20 to 60% by mass, even more preferably 25 to 55% by mass, particularly preferably 30 to 50% by mass, and of these, 35 to 45% by mass is preferred. This facilitates the formation of an adhesive layer that exhibits good adhesion to the adherend, satisfies the physical properties described below, and provides a cured product layer that is excellent in adhesive strength and low dielectric properties. In particular, the resulting cured product layer is likely to exhibit good flex resistance.
[0091] [Component (C): Filler] The adhesive layer according to the present invention preferably contains a filler (hereinafter, sometimes referred to as "filler (C)") as component (C). This allows an appropriate amount of filler (C) to be present in the crosslinked structure formed by materials such as the binder resin (A) and the thermosetting component (B), thereby increasing the strength of the coating and facilitating the production of a cured product that is resistant to external forces such as bending. In particular, this makes it easier to satisfy the physical properties described below and to obtain an adhesive layer that is excellent in flex resistance.
[0092] The shape of the filler (C) may be regular or irregular, but from the viewpoint of film-forming properties, regular shapes are preferred. Regular-shaped fillers include spherical, powdery, fibrous, needle-like, and scale-like. Among these, spherical shapes are preferred, and true spheres are more preferred. This makes it easier for the filler to be uniformly dispersed in the adhesive layer, resulting in excellent film-forming properties and coating strength, making it easier to satisfy the physical properties described below, and making it easier to obtain an adhesive layer with excellent flex resistance. In addition, since the filler is less likely to protrude from the surface of the adhesive layer, it is easier to obtain an adhesive layer with an arithmetic mean surface roughness (Ra) of 200 nm or less, and which has excellent adhesion to the adherend.
[0093] Specific examples of the filler (C) include inorganic fillers such as silica, calcium carbonate, aluminum hydroxide, magnesium hydroxide, clay, talc, titanium dioxide, and zirconia; organic fillers such as acrylic resins, acrylic-styrene copolymers, melamine resins, polycarbonate resins, polyethylene resins, polystyrene resins, benzoguanamine resins, and epoxy resins; and organic-inorganic fillers made of silicon-containing compounds having an intermediate structure between inorganic and organic. Among these, inorganic fillers or organic-inorganic fillers are preferred from the viewpoints of film-forming properties and flex resistance, and inorganic fillers are particularly preferred. Silica fillers are even more preferred from the viewpoint of easily satisfying the physical properties described below. The filler (C) may be used alone or in combination of two or more types.
[0094] The filler (C) may be surface-treated or untreated, but from the viewpoint of film-forming properties and ease of satisfying the physical properties described below, it is preferable that the filler (C) is untreated, which makes it easier to obtain an adhesive layer that is excellent in adhesion to the adherend, low dielectric properties, and flex resistance.
[0095] From the viewpoint of film-forming properties and obtaining an adhesive layer having a good coating surface, the average particle size of the filler (C) is preferably smaller than the thickness of the adhesive layer according to the present invention, and is preferably 0.01 to 10 μm, more preferably 0.05 to 7 μm, even more preferably 0.1 to 4 μm, and even more preferably 0.2 to 3 μm, and of these, 0.3 to 2.5 μm is preferred, and 0.4 to 2 μm is most preferred. This makes it easier to satisfy the physical properties described below, contributing to the formation of an adhesive layer that has excellent adhesion to the adherend, low dielectric properties, and excellent flex resistance. The average particle size of the filler can be measured by centrifugal sedimentation light transmission method.
[0096] The content of the filler (C) is preferably 1 to 80 parts by mass, more preferably 5 to 65 parts by mass, even more preferably 10 to 55 parts by mass, and particularly preferably 15 to 45 parts by mass, relative to 100 parts by mass of the total amount of the components (A), (B), and (C).From the viewpoint of improving the tensile modulus of elasticity, the content is preferably 20 to 40 parts by mass, and even more preferably 25 to 35 parts by mass.This makes it easier to obtain an adhesive layer that satisfies the physical properties described below and has an excellent balance between low dielectric properties and flex resistance.
[0097] The content of the filler (C) in the adhesive layer is preferably 1 to 70% by mass, more preferably 4 to 60% by mass, even more preferably 8 to 50% by mass, and particularly preferably 12 to 40% by mass. From the viewpoint of improving the tensile modulus, it is preferably 16 to 34% by mass, and even more preferably 20 to 28% by mass. This makes it easier to exhibit good adhesion to the adherend, and to obtain a cured product layer that easily satisfies the physical properties described below and has excellent adhesive strength and low dielectric properties. In particular, the resulting cured product layer is more likely to exhibit good flex resistance.
[0098] [Component (D): Thermal Polymerization Initiator] The curing reaction of the adhesive layer according to the present invention preferably involves a thermal polymerization reaction. Therefore, the adhesive layer according to the present invention preferably contains a thermal polymerization initiator (hereinafter, sometimes referred to as "thermal polymerization initiator (D)"). This allows the curing reaction of the adhesive layer to proceed efficiently.
[0099] The thermal polymerization initiator (D) is a compound that generates active species such as radicals or cations that initiate polymerization when heated. Use of the thermal polymerization initiator (D) makes it possible to uniformly initiate a polymerization reaction in the adhesive layer in an environment where heat is easily transferred uniformly throughout the adhesive layer, for example, by heating the adhesive layer by passing it through a heated space maintained at a constant temperature.
[0100] When the adhesive layer-forming composition described below contains an organic solvent, the temperature at which the thermal polymerization initiator (D) has a half-life of 1 minute is preferably higher than the boiling point of the organic solvent, which makes the initiator less likely to react during the adhesive layer production process (particularly the solvent drying step) and more likely to exhibit the desired curing reaction during the annealing treatment step for obtaining a cured product layer.
[0101] The thermal polymerization initiator (D) may be a thermal cationic polymerization initiator or a radical polymerization initiator. The thermal polymerization initiator (D) may be used alone or in combination of two or more.
[0102] The radical polymerization initiator is a compound capable of generating radicals that initiate polymerization when heated, while the thermal cationic polymerization initiator is a compound capable of generating cationic species that initiate polymerization when heated.
[0103] Examples of the thermal cationic polymerization initiator include sulfonium salts, quaternary ammonium salts, phosphonium salts, diazonium salts, and iodonium salts.
[0104] Examples of sulfonium salts include triphenylsulfonium tetrafluoroborate, triphenylsulfonium hexafluoroantimonate, triphenylsulfonium hexafluoroarsinate, tris(4-methoxyphenyl)sulfonium hexafluoroarsinate, and diphenyl(4-phenylthiophenyl)sulfonium hexafluoroarsinate.
[0105] Examples of quaternary ammonium salts include tetrabutylammonium tetrafluoroborate, tetrabutylammonium hexafluorophosphate, tetrabutylammonium hydrogen sulfate, tetraethylammonium tetrafluoroborate, tetraethylammonium p-toluenesulfonate, N,N-dimethyl-N-benzylanilinium hexafluoroantimonate, N,N-dimethyl-N-benzylanilinium tetrafluoroborate, N,N-dimethyl-N-benzylpyridinium hexafluoroantimonate, N,N-diethyl-N-benzyltrifluoromethanesulfonate, N,N-dimethyl-N-(4-methoxybenzyl)pyridinium hexafluoroantimonate, and N,N-diethyl-N-(4-methoxybenzyl)toluidinium hexafluoroantimonate.
[0106] Examples of the phosphonium salt include ethyltriphenylphosphonium hexafluoroantimonate and tetrabutylphosphonium hexafluoroantimonate.
[0107] Examples of iodonium salts include diphenyliodonium hexafluoroarsinate, bis(4-chlorophenyl)iodonium hexafluoroarsinate, bis(4-bromophenyl)iodonium hexafluoroarsinate, and phenyl(4-methoxyphenyl)iodonium hexafluoroarsinate.
[0108] Examples of the radical polymerization initiator include dialkyl peroxides such as benzoyl peroxide, acetyl peroxide, decanoyl peroxide, lauroyl peroxide, cumyl peroxide, and di-t-butyl peroxide; hydroperoxides such as t-butyl peroxybenzoate, t-butylperoxy-2-ethylhexanoate, cumene hydroperoxide, and t-butyl hydroperoxide; t-hexyl peroxy neodecanoate, t-butyl peroxy neodecanoate, t-butyl peroxy neoheptanoate, and t-hexyl peroxy neodecanoate; peroxypivalate, t-butyl peroxypivalate, dilauroyl peroxide, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, disuccinic acid peroxide, t-hexylperoxy-2-ethylhexanoate, t-butylperoxy-2-ethylhexanoate, 1,1-bis(t-hexylperoxy)cyclohexane, 1,1-bis(t-butylperoxy)cyclohexane, t-hexylperoxyisopropyl monocarbonate, t-butylperoxy Oxymaleic acid, t-butylperoxy 3,5,5-trimethylhexanoate, t-butylperoxy isopropyl monocarbonate, t-butylperoxy 2-ethylhexyl monocarbonate, t-butylperoxy laurate, t-hexylperoxybenzoate, t-butylperoxy acetate, t-butylperoxybenzoate, n-butyl 4,4-bis(t-butylperoxy)valerate, dicumyl peroxide, di-t-hexyl peroxide, di-t-butyl peroxide, p-methyl peroxide (organic) peroxide-based thermal polymerization initiators such as ethane hydroperoxide; and azo-based thermal polymerization initiators such as 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(4-cyanovaleronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(methyl isobutyrate), and 1,1'-azobis(1-cyclohexanecarbonitrile).
[0109] The thermal polymerization initiator (D) is preferably a thermal cationic polymerization initiator, and particularly preferably a sulfonium salt-based thermal cationic polymerization initiator. This allows the adhesive layer according to the present invention to form a desired crosslinked structure and exhibit the properties described below, making it easier to obtain a cured layer with excellent adhesive strength and low dielectric properties. In particular, the obtained cured layer exhibits good flex resistance.
[0110] The content of the thermal polymerization initiator (D) is preferably 0.1 to 20 parts by mass, more preferably 0.5 to 15 parts by mass, even more preferably 1 to 10 parts by mass, and particularly preferably 2 to 5 parts by mass, relative to 100 parts by mass of the total amount of the components (A), (B), and (C). This makes it easier to obtain an adhesive layer that satisfies the physical properties described below and that has an excellent balance between low dielectric properties and flex resistance.
[0111] When the adhesive layer contains a thermal polymerization initiator (D), the content thereof in the adhesive layer is preferably 0.1 to 10 mass%, more preferably 0.5 to 8 mass%, particularly preferably 1 to 6 mass%, and even more preferably 2 to 4 mass%. This makes it easier to form a desired crosslinked structure and exhibit the physical properties described below, and more efficiently form a cured product layer that has excellent adhesive strength and low dielectric properties. In particular, the resulting cured product layer exhibits good flex resistance.
[0112] [Component (E): Silane Coupling Agent] The adhesive layer according to the present invention preferably contains a silane coupling agent (hereinafter sometimes referred to as "silane coupling agent (E)") as component (E). This can improve adhesion to the adherend, making it easier to form an adhesive layer with higher adhesive strength.
[0113] As the silane coupling agent (E), known silane coupling agents can be used, among which organosilicon compounds having at least one alkoxysilyl group in the molecule are preferred.
[0114] Examples of the silane coupling agent (E) include silane coupling agents having a (meth)acryloyl group, silane coupling agents having a vinyl group, silane coupling agents having an epoxy group, silane coupling agents having a styryl group, silane coupling agents having an amino group, silane coupling agents having an isocyanurate skeleton, silane coupling agents having a ureido group, silane coupling agents having a halogen atom, silane coupling agents having a mercapto group, silane coupling agents having an isocyanate group, silane coupling agents having an allyl group, silane coupling agents having a hydroxyl group, and silane coupling agents having an acid anhydride structure. Among these, from the viewpoint of easily obtaining an adhesive layer that gives a cured product layer with higher adhesive strength by thermal curing, silane coupling agents having an epoxy group, silane coupling agents having an isocyanate group, silane coupling agents having an allyl group, silane coupling agents having a hydroxyl group, silane coupling agents having an isocyanurate skeleton, silane coupling agents having a mercapto group, and silane coupling agents having an acid anhydride structure are preferred, silane coupling agents having an epoxy group, silane coupling agents having a hydroxyl group, and silane coupling agents having an acid anhydride structure are particularly preferred, and silane coupling agents having an acid anhydride structure are preferred. The silane coupling agent (E) can be used alone or in combination of two or more.
[0115] When the adhesive layer according to the present invention contains a silane coupling agent (E), the content thereof in the adhesive layer is preferably 0.01 to 5 mass%, more preferably 0.04 to 3 mass%, even more preferably 0.08 to 1 mass%, particularly preferably 0.10 to 0.70 mass%, and of these, 0.12 to 0.40 mass% is preferred. This makes it easier to exhibit the physical properties described below and to form a cured material layer that is excellent in adhesive strength and low dielectric properties. In particular, the resulting cured material layer exhibits good flex resistance.
[0116] [Component (F): Crosslinking Agent] The adhesive layer of the adhesive sheet of the present invention preferably contains, as component (F), a crosslinking agent capable of reacting with components (A) and (B) (hereinafter, sometimes referred to as "crosslinking agent (F)"). This makes it easier to obtain an adhesive layer that easily satisfies the physical properties described below, and also makes it easier to form a cured layer having the desired crosslinking density by heat treatment.
[0117] The crosslinking agent (F) is preferably one that undergoes a thermosetting reaction upon heat treatment, and is particularly preferably a compound that can react well with the aforementioned component (A). Specifically, the crosslinking agent (F) is preferably one that has a reactive group or reactive site that is reactive with the reactive functional group in the binder resin (A).
[0118] Examples of the crosslinking agent (F) include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, amine-based crosslinking agents, melamine-based crosslinking agents, metal chelate-based crosslinking agents, metal salt-based crosslinking agents, ammonium salt-based crosslinking agents, hydrazine-based crosslinking agents, aldehyde-based crosslinking agents, oxazoline-based crosslinking agents, metal alkoxide-based crosslinking agents, and aziridine-based crosslinking agents. Among these, isocyanate-based crosslinking agents, epoxy-based crosslinking agents, and metal chelate-based crosslinking agents are preferred from the viewpoint of storage stability, and metal chelate-based crosslinking agents are particularly preferred from the viewpoint of easily satisfying the physical properties described below. The crosslinking agent (F) can be used alone or in combination of two or more.
[0119] The isocyanate crosslinking agent is a compound having two or more isocyanate groups in the molecule. Examples of the isocyanate crosslinking agent include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, hydrogenated tolylene diisocyanate, hydrogenated xylene diisocyanate, 1,5-pentamethylene diisocyanate, 1,6-hexamethylene diisocyanate, diphenylmethane-4,4-diisocyanate, isophorone diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, tetramethylxylylene diisocyanate, 1,5-naphthalene diisocyanate, triphenylmethane triisocyanate, adducts of these polyisocyanate compounds with polyol compounds such as trimethylolpropane, and biuret and isocyanurate forms of these polyisocyanate compounds.
[0120] Epoxy crosslinking agents are compounds having two or more epoxy groups in the molecule. Examples of epoxy crosslinking agents include 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, N,N,N',N'-tetraglycidyl-m-xylylenediamine, ethylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane diglycidyl ether, diglycidylaniline, and diglycidylamine.
[0121] The metal chelate crosslinking agent is a chelate compound having a metal ion that functions as a crosslinking point. As the metal chelate crosslinking agent, for example, a metal chelate compound whose metal ion is aluminum ion, zirconium ion, titanium ion, zinc ion, iron ion, tin ion, etc. can be used. Among these, aluminum chelate compounds are preferred.
[0122] Examples of aluminum chelate compounds include aluminum tris(acetylacetonate), acetylacetonate aluminum bis(ethylacetoacetate), diisopropoxyaluminum monooleylacetoacetate, and monoisopropoxyaluminum bisoleylacetoacetate.
[0123] When the adhesive layer contains a crosslinking agent (F), the content thereof in the adhesive layer is preferably 0.01 to 10 mass%, more preferably 0.05 to 5 mass%, even more preferably 0.1 to 2 mass%, particularly preferably 0.15 to 1 mass%, and of these, preferably 0.2 to 0.7 mass%, and most preferably 0.22 to 0.4 mass%. This makes it easier to satisfy the physical properties described below, and a cured product layer excellent in adhesive strength and low dielectric properties is formed, which exhibits good flex resistance while exhibiting desired dielectric properties.
[0124] [Other Components] The adhesive layer according to the present invention may contain components other than those described above (other components) to the extent that the effects of the present invention are not impaired. Examples of other components include additives such as ultraviolet absorbers, antistatic agents, light stabilizers, antioxidants, oxygen absorbers, infrared absorbers, colorants, rust inhibitors, tackifiers, resin stabilizers, fillers, extenders, dispersants, and softeners. These can be used alone or in combination of two or more. When the raw material composition contains these additives, the content thereof can be appropriately determined depending on the purpose.
[0125] [Dispersant] The adhesive layer according to the present invention preferably contains a dispersant, which makes it possible to easily and uniformly disperse the filler (C) in the adhesive layer-forming composition described below, and as a result, it is easy to form a high-quality adhesive layer in which the filler (C) is uniformly dispersed.
[0126] Examples of dispersants include monocarboxylic acids such as lauric acid, myristic acid, palmitic acid, margaric acid, and stearic acid; aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, orthophthalic acid, and 2,6-naphthalenedicarboxylic acid; dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, sebacic acid, dodecanedicarboxylic acid, and azelaic acid; dibasic acids having 12 to 28 carbon atoms such as dimer acid; 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, 4-methylhexahydrophthalic anhydride, and 3-methylhexahydro anhydride. Examples of suitable dicarboxylic acids include alicyclic dicarboxylic acids such as phthalic acid, 2-methylhexahydrophthalic anhydride, hydrogenated dicarboxy bisphenol A, hydrogenated dicarboxy bisphenol S, dimer acid, hydrogenated dimer acid, hydrogenated naphthalenedicarboxylic acid, and tricyclodecane dicarboxylic acid; hydroxycarboxylic acids such as hydroxybenzoic acid and lactic acid; trivalent or higher carboxylic acids such as trimellitic anhydride and pyromellitic anhydride; unsaturated dicarboxylic acids such as fumaric acid and maleic acid; carboxylic acid diols such as dimethylolbutanoic acid and dimethylolpropionic acid; and Disperbyk-2155 (trade name: manufactured by BYK Corporation).
[0127] The amount of dispersant used is preferably 0.1 to 20 parts by mass, more preferably 0.5 to 15 parts by mass, even more preferably 1.0 to 10 parts by mass, and particularly preferably 1.4 to 5 parts by mass, per 100 parts by mass of the filler (C). This makes it easier to uniformly disperse the filler in the adhesive, and thus makes it possible to obtain an adhesive layer that is more likely to exhibit the physical properties described below. This in turn makes it possible to achieve excellent flex resistance while also having excellent dielectric properties.
[0128] (Preparation of Adhesive Layer-Forming Composition) The adhesive layer-forming composition can be prepared by mixing a binder resin (A), a thermosetting component (B), a filler (C), a thermal polymerization initiator (D), a silane coupling agent (E), a crosslinking agent (F), and a dispersant as another component. Taking into consideration handleability, coatability, and the like, an organic solvent may be contained. Examples of the solvent to be used include aromatic hydrocarbon solvents such as benzene and toluene; ester solvents such as ethyl acetate and butyl acetate; ketone solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; aliphatic hydrocarbon solvents such as n-pentane, n-hexane, and n-heptane; and alicyclic hydrocarbon solvents such as cyclopentane, cyclohexane, and methylcyclohexane. These solvents can be used alone or in combination of two or more. The solvent content can be determined appropriately taking into consideration coatability, etc.
[0129] [Formation of Adhesive Layer] The adhesive layer can be formed using a composition for forming an adhesive layer by applying a predetermined amount of the composition for forming an adhesive layer onto a process sheet (or a release sheet described later) and drying the resulting coating.
[0130] Conventional process sheets can be used. Examples of process sheet substrates include resin films and paper. Examples of resins for resin films include polyethylene terephthalate, polyethylene, polypropylene, polybutene, polybutadiene, polymethylpentene, polyvinyl chloride, vinyl chloride copolymers, polybutylene terephthalate, polyurethane, ethylene-vinyl acetate copolymers, ionomer resins, ethylene (meth)acrylic acid copolymers, polystyrene, polycarbonate, fluororesins, low-density polyethylene, linear low-density polyethylene, and triacetyl cellulose. Examples of paper include fine paper, coated paper, glassine paper, and laminated paper. From the perspective of the SDGs, the process sheets may be made of materials with a high biomass content, recyclable or reusable materials, or recycled or reused materials. These materials may be used alone or in combination.
[0131] There is no particular limitation on the thickness of the process sheet, but it is usually about 20 to 150 μm.
[0132] Examples of methods for applying the adhesive layer-forming composition include spin coating, spray coating, bar coating, knife coating, roll coating, blade coating, die coating, and gravure coating.
[0133] Methods for drying the coating film include conventionally known drying methods such as hot air drying, heated roll drying, infrared irradiation, etc. The coating film can be dried, for example, at a drying temperature of 80 to 150°C for a drying time of 30 seconds to 5 minutes.
[0134] The thickness of the adhesive layer according to the present invention is usually 1 to 100 μm, preferably 4 to 80 μm, more preferably 8 to 60 μm, even more preferably 12 to 50 μm, particularly preferably 15 to 40 μm, and of these, preferably 18 to 30 μm. This makes it easier to achieve suitable adhesive strength and the physical properties described below, and to achieve an excellent balance between low dielectric properties and flex resistance.
[0135] The adhesive layer according to the present invention preferably satisfies the formula: Y / X<1, more preferably: Y / X<0.5, even more preferably: Y / X<0.2, particularly preferably: Y / X<0.1, more preferably: Y / X<0.08, and even more preferably: Y / X<0.07, where X (μm) is the thickness of the adhesive layer and Y (μm) is the average particle size of the filler (C). The lower limit of Y / X is not particularly limited, but is usually greater than 0, preferably 0.001 or greater, more preferably 0.004 or greater, even more preferably 0.008 or greater, and particularly preferably 0.01 or greater. This makes it easier to achieve suitable adhesive strength and the physical properties described below, and to achieve an excellent balance between low dielectric properties and flex resistance.
[0136] In this manner, an adhesive sheet having a layer structure of a process sheet (or release sheet) / adhesive layer can be obtained. A release sheet may be placed on the surface of the adhesive layer to protect the surface of the adhesive layer when storing or transporting the adhesive sheet. The same release sheets as those described above can be used. The process sheet and release sheet are peeled and removed when used. When process sheets or release sheets are provided on both sides of the adhesive layer, from the viewpoint of handleability, it is preferable that there be a difference in peel strength when peeling one process sheet (or release sheet) and the other process sheet (or release sheet).
[0137] In this specification, the release surface of the process sheet and the release sheet refers to the surface of the release sheet that has releasability, and includes both a surface that has been subjected to a release treatment and a surface that exhibits releasability even without a release treatment. It is preferable that the release surface of the release sheet (particularly the surface that contacts the adhesive layer) has been subjected to a release treatment. Examples of release agents used in the release treatment include alkyd-based, silicone-based, fluorine-based, rubber-based, long-chain alkyl-based, unsaturated polyester-based, polyolefin-based, and wax-based release agents, with non-silicone-based release agents being preferred.
[0138] (Curing of Adhesive Layer) The adhesive layer of the adhesive sheet of the present invention is cured by heating to form a cured layer. The curing conditions for the adhesive layer can be determined appropriately depending on the curable components contained in the adhesive layer. The heating temperature is usually 140°C or higher, preferably 150 to 180°C. The heating time is usually 0.5 to 3 hours, preferably 1 to 2 hours.
[0139] The adhesive sheet of the present invention has the following properties. (1) Arithmetic mean surface roughness (Ra) The arithmetic mean surface roughness (Ra) of the adhesive layer surface of the adhesive sheet of the present invention is 200 nm or less, preferably 0 to 150 nm, more preferably 0.1 to 100 nm, even more preferably 1 to 75 nm or less, particularly preferably 2 to 50 nm, and of these, 48 nm is preferable. This gives the adhesive layer a good coating surface with low transmission loss. The arithmetic mean surface roughness (Ra) of the adhesive layer surface, which facilitates the desired adhesive strength and particularly facilitates the development of excellent flex resistance, is the average of the absolute values of the heights of the roughness curves over the reference length specified in ISO 25178, and can be measured by the method described in the examples.
[0140] (2) Dielectric Constant: The adhesive layer of the adhesive sheet of the present invention has excellent low dielectric properties. The dielectric constant of the cured material layer obtained by heat-treating the adhesive layer of the adhesive sheet of the present invention at 170°C for 2 hours at 23°C and a frequency of 10 to 40 GHz is preferably 3.0 (F / m) or less, more preferably 2.8 (F / m) or less, and even more preferably 2.7 (F / m) or less. There is no particular lower limit for the dielectric constant, but it is usually 2.00 (F / m) or more. The dielectric constant of the cured material layer at 23°C and a frequency of 10 to 40 GHz can be measured by the method described in the Examples.
[0141] (3) Dielectric Loss Tangent The cured product layer obtained by heat-treating the adhesive layer provided in the adhesive sheet of the present invention at 170°C for 2 hours has a dielectric loss tangent of 0.005 or less, preferably 0.0045 or less, and more preferably 0.004 or less at 23°C and a frequency of 10 to 40 GHz. Therefore, when the adhesive sheet of the present invention is used as a material for forming an insulating layer in an electronic device, the insulating layer will have low transmission loss. The dielectric loss tangent of the cured product layer at 23°C and a frequency of 10 to 40 GHz can be measured by the method described in the Examples.
[0142] (4) Gel Fraction The gel fraction of the adhesive constituting the adhesive layer of the adhesive sheet of the present invention is preferably 10 to 70%, more preferably 13 to 60%, even more preferably 16 to 50%, and particularly preferably 20 to 40%. This facilitates the formation of an adhesive layer that is easy to handle and has excellent curing properties and adhesion to the adherend.
[0143] The gel fraction of the cured product layer obtained by heat-treating the adhesive layer of the adhesive sheet of the present invention at 170°C for 2 hours is preferably 40 to 90%, more preferably 45 to 85%, even more preferably 50 to 80%, particularly preferably 50 to 80%, and of these, 50 to 80% is preferred. This ensures that the cured product layer has a sufficiently formed crosslinked structure and is likely to exhibit particularly high adhesive strength. Therefore, the adhesive layer that provides such a cured product layer will have excellent flex resistance. The gel fractions of the adhesive layer and the cured product layer can be calculated using the method described in the Examples.
[0144] (5) Rate of Increase in Gel Fraction When the gel fraction of the adhesive layer of the adhesive sheet of the present invention before curing is α (%) and the gel fraction of the cured layer obtained by curing the adhesive layer is β (%), the rate of increase in gel fraction (%), expressed by the formula: [(β-α) / α] × 100, is preferably 60% or more, more preferably 80% or more, even more preferably 100% or more, and particularly preferably 110% or more, with 120% or more being preferred and 130% or more being most preferred. The upper limit of this rate of increase is not particularly limited, but is preferably 800% or less, more preferably 600% or less, even more preferably 400% or less, and particularly preferably 350% or less. From the viewpoint of a tendency for the tensile modulus to increase, it is preferably 300% or less, and particularly preferably 250% or less. This tends to result in an excellent balance between low dielectric properties and flex resistance. The cured layer formed by curing the adhesive layer typically has more crosslinked structures than the adhesive layer itself. Therefore, the gel fraction of the cured product layer is usually greater than that of the adhesive layer. When the cured product of the adhesive layer functions as an adhesive member, a protective member, an insulating member, or the like, it is preferable that the curing reaction of the cured product has progressed sufficiently.
[0145] (6) Tensile Modulus (E') The tensile modulus at 25°C of the cured material layer obtained by heat-treating the adhesive layer provided in the adhesive sheet of the present invention at 170°C for 2 hours is not particularly limited, but is preferably 0.5 to 10 GPa, more preferably 1.0 to 7.0 GPa, even more preferably 1.5 to 5.0 GPa, particularly preferably 1.6 to 3.0 GPa, and of these, 1.7 to 2.0 GPa is preferred. This tends to result in excellent dielectric properties and flex resistance in the high frequency band. The tensile modulus at 25°C of the cured material layer obtained by heat-treating the adhesive layer at 170°C for 2 hours can be measured by the method described in the Examples.
[0146] The thermosetting adhesive sheet of the present invention is suitable for use as an adhesive sheet for electronic devices. For example, the adhesive layer constituting the thermosetting adhesive sheet of the present invention can be used to bond various components in an electronic device or to form an insulating layer for a conductive layer (circuit, etc.) in an electronic device. Examples of electronic devices include communication devices such as smartphones and tablet terminals.
[0147] The thermosetting adhesive sheet of the present invention is suitable for use as an adhesive sheet for a coverlay film. A coverlay film is a laminated film used, for example, to protect the surface of a flexible printed wiring board, and typically has an insulating resin layer and an adhesive layer. For example, a coverlay film can be produced by (thermo)compression bonding the adhesive layer constituting the thermosetting adhesive sheet of the present invention to an insulating resin film.
[0148] 2) Laminate The second aspect of the present invention is a laminate comprising a conductive layer and an insulating layer formed on the conductive layer, wherein the insulating layer is a cured layer formed by curing the adhesive layer of the thermosetting adhesive sheet of the present invention.
[0149] Examples of conductive layers include conductive layers (circuits, etc.) in electronic devices, such as layers that form wiring that serves as a conductor for electrical signals in a printed wiring board obtained from a metal-clad laminate.
[0150] Examples of metals that can be used as raw materials for the conductive layer include copper, aluminum, silver, gold, zinc, nickel, tin, iron, alloys containing these, etc. Among these, copper or alloys containing copper are particularly preferred in terms of conductivity.
[0151] The thickness of the conductive layer according to the present invention is preferably 1 to 1000 μm, more preferably 10 to 800 μm, still more preferably 40 to 600 μm, particularly preferably 80 to 500 μm, and of these, preferably 120 to 400 μm.
[0152] The laminate of the present invention uses the adhesive sheet of the present invention and has both excellent low dielectric properties and flex resistance.
[0153] 3) Manufacturing method of laminate The third aspect of the present invention is a manufacturing method of the laminate of the present invention, which comprises the steps of: (I) laminating an adhesive layer provided in the thermosetting adhesive sheet of the present invention onto a conductive layer to obtain a laminate; and (II) heating the laminate to a predetermined temperature to cure the adhesive layer of the thermosetting adhesive sheet. The manufacturing method of the present invention will be described with reference to FIG.
[0154] First, as shown in Figure 1(a), a thermosetting adhesive sheet 10 according to the present invention is prepared, which has release sheets 2a, 2b on both sides of an adhesive layer 1. The release sheets 2a, 2b are to be peeled and removed when in use (when producing a laminate).
[0155] 1(b), after peeling off the release sheet 2a, the conductive layer 3 is bonded to the exposed surface of the adhesive layer 1. Then, the release sheet 2b is peeled off and an insulating resin layer 4 is formed on the exposed surface of the adhesive layer 1, thereby obtaining a laminate 20 (Step I-1). The insulating resin layer 4 can be formed by applying an insulating resin layer-forming composition to the exposed surface of the adhesive layer 1 and drying the resulting coating, by bonding an insulating resin film to the exposed surface of the adhesive layer 1, or by other methods.
[0156] Examples of materials for the insulating resin layer 4 include polyimides obtained by reacting tetracarboxylic dianhydride with diamine; modified polyimides obtained by modifying polyimide with other resins, such as phenolic resin-modified polyimide, novolac resin-modified polyimide, polyvinylphenol-modified polyimide, polyurethane-modified polyimide containing phenolic hydroxyl groups, and polyurea-modified polyimide having phenolic hydroxyl groups. From the perspective of the SDGs, the material constituting the insulating resin layer may be a material with a high biomass content, a recyclable or reusable material, or a recycled or reused material. These materials may be used alone or in combination of two or more.
[0157] The thickness of the insulating resin layer 4 according to the present invention is preferably 1 to 100 μm, more preferably 4 to 80 μm, even more preferably 8 to 60 μm, particularly preferably 16 to 40 μm, and of these, preferably 20 to 30 μm.
[0158] Thereafter, as shown in Figure 1(c), the laminate 20 is heated and pressed to cure the adhesive layer 1, thereby obtaining the laminate 30 according to the present invention as a cured layer 5. Any method can be used to heat and cure the adhesive layer 1. For example, a hot press or a hot roll device can be used. According to the production method of the present invention, the laminate according to the present invention can be efficiently produced.
[0159] The above-described embodiments have been described to facilitate understanding of the present invention, and are not intended to limit the present invention. Therefore, each element disclosed in the above embodiments is intended to include all design modifications and equivalents that fall within the technical scope of the present invention.
[0160] In this specification, when it is stated that "α to β" (α and β are any numerical values), it means "not less than α and not more than β" and also means "preferably greater than α" or "preferably smaller than β" unless otherwise specified. Furthermore, when it is stated that "not less than α" (α is any numerical value), it also means "preferably greater than α" unless otherwise specified, and when it is stated that "not more than β" (β is any numerical value), it also means "preferably smaller than β" unless otherwise specified.
[0161] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0162] [Compounds used in Examples and Comparative Examples] (1-1) Binder resin (A1): Acid-modified α-olefin polymer (manufactured by Mitsui Chemicals, Inc., trade name: UNISTOL H-200) (1-2) Binder resin (A2): Acid-modified styrene-based elastomer (manufactured by Kraton Polymers, trade name: FG-1901) (2-1) Thermosetting component (B1a): Diallyl compound having an isocyanurate skeleton (manufactured by Shikoku Chemicals Corporation, trade name: L-DAIC) (2-2) Thermosetting component (B2a): Vinylbenzyl-modified polyphenylene ether (manufactured by Mitsubishi Gas Chemical Company, Inc., trade name: OPE-2St 2200) (3-1) Filler (C1): High-purity spherical silica fine particles (average particle size: 1.5 μm, manufactured by Nippon Shokubai Co., Ltd., trade name: Seahoster KE-S150) (3-2) Filler (C2): High-purity spherical silica particles (average particle size: 0.5 μm, manufactured by Nippon Shokubai Co., Ltd., trade name: Seahoster KE-S50) (3-3) Irregular silica (C3) (average particle size: 2.7 μm, manufactured by Fuji Silysia Chemical Co., Ltd., trade name: Sylysia 530) (3-4) Filler (C4): Functionalized spherical silica particles (average particle size: 1.5 μm, manufactured by Nippon Shokubai Co., Ltd., trade name: Seahoster KE-E150) (4) Thermal polymerization initiator (D1): Sulfonium salt-based thermal cationic polymerization initiator (manufactured by Sanshin Chemical Co., Ltd., trade name: San-Aid SI-B3) (5) Silane coupling agent (E1): 3-trimethoxysilylpropylsuccinic anhydride (manufactured by Shin-Etsu Chemical Co., Ltd., trade name: X-12-967C) Acid anhydride (6) Crosslinking agent (F1): Tris(2,4-pentanedionato)aluminum(III) (manufactured by Soken Chemical & Engineering Co., Ltd., trade name: M-5A) (7) Dispersant: (manufactured by BYK, trade name: DISPAERBYK2155)
[0163] (Examples 1 to 4, Comparative Examples 1 to 4) 100 parts by weight of binder resin (A1) (solid content equivalent; the same applies hereinafter), 130 parts by weight of thermosetting component (B1a), 250 parts by weight of thermosetting component (B2a), 100 parts by weight of filler (C1), 15 parts by weight of thermal polymerization initiator (D1), 1.0 part by weight of silane coupling agent (E1), 1.5 parts by weight of crosslinking agent (F1), and 1.7 parts by weight of dispersant were mixed together with a solvent to a uniform mixture and thoroughly stirred to prepare an adhesive layer-forming composition. Next, the adhesive layer-forming composition was applied using a coater to a heavy-release release sheet R1, one side of which had been treated with a rubber-based release agent (non-silicone-based release agent). The resulting coating was then dried at 100°C for 2 minutes to form a coating layer with a thickness of 25 μm. Next, the coating layer on the release sheet R1 obtained above was laminated to a light-release type release sheet R2, which was a polyethylene terephthalate film with one side treated with a rubber-based release agent (non-silicone-based release agent), so that the release-treated surface of the release sheet R2 was in contact with the coating layer, and the resulting mixture was aged for 7 days at 23°C and 50% RH. This produced an adhesive sheet with a 25 μm-thick adhesive layer, i.e., a thermosetting adhesive sheet consisting of release sheet R1 / adhesive layer (thickness: 25 μm) / release sheet R2.
[0164] The thickness of the adhesive layer was measured in accordance with JIS K 7130 using a constant pressure thickness gauge (manufactured by Teclock Corporation, product name "PG-02"). Regarding the release strength of Release Sheet 1 and Release Sheet R2 in the obtained thermosetting adhesive sheet, it was confirmed that Release Sheet R1 had a greater release strength than Release Sheet R2.
[0165] (Examples 2 to 4, Comparative Examples 1 to 4) Adhesive layers were formed in the same manner as in Example 1, except that the composition for forming the adhesive layer was changed to the formulation shown in Table 1 below, to produce adhesive sheets of Examples 2 to 4 and Comparative Examples 1 to 4.
[0166]
[0167] (Laminate Preparation) The release sheet R2 was peeled off from the adhesive sheet obtained in the Examples or Comparative Examples to expose the adhesive layer. The resulting adhesive sheet was then placed on copper foil (Kansai Electronics Co., Ltd., product name: C1100P, glossy, thickness: 300 μm). The release sheet R1 was then peeled off from the adhesive layer, and a modified polyimide (MPI) film (PI Advanced Materials, Korea, product number: PI FG100, thickness: 25 μm) was attached to the exposed adhesive layer to obtain a laminate (MPI film / adhesive layer / copper foil layer configuration). The laminate was subjected to a pre-annealing treatment (1 MPa, 160°C, 5 minutes) using a vacuum laminator (manufacturer: Nikko Materials Co., Ltd., model number: V130), followed by an annealing treatment (170°C, 2 hours) under pressure-free conditions. As a result of the above, laminates having a layer structure of MPI film / cured material layer / copper foil, in which the adhesive layer of the adhesive sheet of Examples 1 to 4 and Comparative Examples 1 to 4 had a cured material layer, were obtained.
[0168] [Evaluation of Physical Properties] The obtained adhesive sheet samples were evaluated for various physical properties according to the following (Test and Evaluation Methods).
[0169] (1) Evaluation of film formability The adhesive layer-forming compositions of the Examples and Comparative Examples were applied to a release sheet R1 using a coater to obtain coating films, which were then dried at a drying temperature of 100°C for 2 minutes to form coating layers with a thickness of 25 µm. A coating film with good appearance, with no visible cissing marks, streaks, or point-like defects, was rated as ◯; a coating film with poor appearance, with no visible cissing, streaks, or point-like defects, was rated as ×. The results are shown in Table 2.
[0170] (2) Arithmetic Mean Surface Roughness (Ra) The surface roughness of the adhesive layer [arithmetic mean surface roughness (Ra; nm)] was measured using a surface roughness measuring device in accordance with ISO 25178. The results are shown in Table 2.
[0171] (3) Gel Fraction of Adhesive Layer The adhesive sheet obtained in each of the Examples and Comparative Examples was cut to a size of 80 mm x 80 mm, and both release sheets were peeled off to obtain an adhesive layer. The resulting adhesive layer was then wrapped in a polyester mesh (mesh size 200) whose mass had been measured in advance to prepare a test sample. The test sample was left to stand for 24 hours in an environment at 23°C and 50% RH, and then its mass was weighed using a precision balance. Based on the obtained measurement value, the mass of the adhesive layer before immersion (M1) was calculated. Next, the test sample was immersed in 0.2 L of toluene at room temperature (23°C) for 72 hours. After immersion, the test sample was removed and dried in an oven at 100°C for 2 hours, and then left to stand for 24 hours in an environment at 23°C and 50% RH. The mass of the dried test sample was weighed using a precision balance. Based on the obtained measurement value, the mass of the adhesive layer after immersion and drying (M2) was calculated. The gel fraction of the adhesive layer was calculated from the values of M1 and M2 using the following formula: The results are shown in Table 2.
[0172]
[0173] (4) Gel fraction of cured product layer The adhesive sheets obtained in the Examples and Comparative Examples were cut into pieces measuring 80 mm length x 80 mm width, and then heated in an oven at 170°C for 2 hours. The release sheet was peeled off to obtain a cured product layer, and the gel fraction of the cured product was calculated in the same manner as above. The results are shown in Table 2.
[0174] (5) Gel Fraction Increase Rate The gel fraction increase rate (%) was calculated using the gel fraction α (%) calculated in (3) above and the gel fraction β (%) of the same sample after curing calculated in (4) according to the following formula. The results are shown in Table 2.
[0175]
[0176] (6) Dielectric Constant (Dk) and Dielectric Loss Tangent (Df) The adhesive sheets obtained in the Examples and Comparative Examples were cut to a size of 80 mm length x 80 mm width, and then annealed at 170°C for 2 hours to form the adhesive layer into a cured product layer. Next, both release sheets were peeled off to obtain a cured product layer sample. The dielectric constant and dielectric loss tangent of this sample were measured using a cavity resonator type dielectric constant measuring device (TE mode, frequencies: 10 GHz, 28 GHz, 40 GHz) in accordance with JIS R1641 IPC-TM650 2.5.5.13. Analyzer: Model MS46122B manufactured by Anritsu Corporation. Resonator: 10, 28, 40 GHz manufactured by AET Corporation.
[0177] (7) Tensile Modulus (E') The adhesive layer of the adhesive sheet obtained in the Examples or Comparative Examples was laminated to a thickness of 200 μm, and the resulting adhesive layer (thickness: 200 μm) was cut into a size of 20 mm length x 5 mm width. Using a vacuum laminator (manufactured by Nikko Materials Co., Ltd., model number: V130), the sample was pre-annealed (1 MPa, 160°C, 5 minutes), and then annealed (170°C, 2 hours) under pressure-free conditions to obtain a measurement sample. The resulting measurement sample was measured for the tensile modulus [E' (GPa)] of the cured layer at 25°C using a dynamic viscoelasticity measuring device (manufactured by Netsch, model: DMA 242E Artemis, mode: tension, frequency: 1 Hz, measurement sample chuck distance: 10 mm, measurement sample width: 5 mm).
[0178] (8) Flexibility Test The laminate having the above-described layer structure of MPI film / cured product layer / copper foil was repeatedly bent under the following conditions using a sheet-shaped no-load U-shaped expansion / contraction tester (manufactured by Yuasa System Co., Ltd., product name "CL09-typeD01-FSC90"). Thereafter, the bent portion was visually inspected, and the flexibility was evaluated according to the following evaluation criteria. Test configuration: MPI film / cured product layer / copper foil Minimum bend diameter: 3 mmφ Number of bends: 100,000 times Sample size: 50 mm x 200 mm Test temperature: 23°C
[0179] <Evaluation criteria> ◯: No lines due to flexion marks were present in the bent portion. Δ: Lines due to flexion marks were present in the bent portion, and the lines were visible when viewed from the front and from a 60° diagonal direction. ×: The cured product layer (adhesive layer) was broken.
[0180] (9) Adhesive Strength The adhesive layer exposed by peeling off the release sheet R2 from the adhesive sheet obtained in the Examples or Comparative Examples was transferred to the glossy side of copper foil (manufactured by Kansai Electronics Co., Ltd., product name: C1100P glossy, thickness 300 μm) at a pressure of 0.2 MPa using a pressure-sensitive adhesive rubber roll heated to 100°C, and cut into a test piece measuring 1.0 cm wide x 10 cm long. Next, the release sheet R1 of the test piece was peeled off, and the exposed adhesive layer was attached to the MPI film surface of the above-mentioned MPI film laminate attached to an aluminum plate via a pressure-sensitive adhesive layer at a pressure of 0.2 MPa using a pressure-sensitive adhesive rubber roll heated to 100°C, and this was used as a test sample (MPI film / adhesive layer / copper foil laminate). The test sample was subjected to a pre-annealing treatment (1 MPa, 160°C, 1 minute) using a vacuum laminator (Nikko Materials Co., Ltd., model number: V130) and then to an annealing treatment (170°C, 2 hours) under pressure-free conditions to obtain a measurement sample (MPI film / cured material layer / copper foil laminate). The measurement sample was allowed to stand for 24 hours in an environment of 23°C and 50% RH, and then the adhesive strength was measured using a tensile tester under conditions of 90° peel and a peel rate of 50 mm / min.
[0181] The above measurement results and evaluation results are shown in Table 2 below.
[0182]
[0183] The above table reveals the following: The thermosetting adhesive sheets of Examples 1 to 4, which contained components (A), (B), and (C), had an arithmetic mean surface roughness (Ra) of the adhesive layer surface of 200 nm or less, a dielectric dissipation factor of the cured product layer at 23°C and 10 to 40 GHz of 0.005 or less, and a gel fraction of the cured product layer of 40% or more, had excellent flex resistance and high adhesive strength.
[0184] On the other hand, the thermosetting adhesive sheet of Comparative Example 1 had poor film-forming properties, and it was not possible to measure various physical properties of the cured product layer, such as the dielectric constant, dielectric dissipation factor, and tensile modulus. The thermosetting adhesive sheet of Comparative Example 2 had insufficient curing of the adhesive layer, a low rate of increase in gel fraction of the adhesive layer before and after curing, and poor flex resistance. The thermosetting adhesive sheet of Comparative Example 3 had a low tensile modulus of the cured product layer, and the cured product layer broke in the flex test, resulting in poor flex resistance. Furthermore, the thermosetting adhesive sheet of Comparative Example 4 had poor dielectric properties at 10 to 40 GHz.
[0185] DESCRIPTION OF SYMBOLS 1... adhesive layer 2a, 2b... release sheet 3... conductive layer 4... insulating resin layer 5... cured product layer 10... thermosetting adhesive sheet 20... laminate 30... laminate
Claims
1. A thermosetting adhesive sheet having an adhesive layer, the adhesive layer being a layer containing the following components (A), (B), and (C); the adhesive layer surface has an arithmetic mean surface roughness (Ra) of 200 nm or less; the adhesive layer is heat-treated at 170°C for 2 hours to obtain a cured material layer, which has a dielectric loss tangent of 0.005 or less at 23°C and a frequency of 10 to 40 GHz; and the adhesive layer is heat-treated at 170°C for 2 hours to obtain a cured material layer, which has a gel fraction of 40% or more. Component (A): Binder resin Component (B): Thermosetting component Component (C): Filler 2. The thermosetting adhesive sheet according to claim 1, wherein the gel fraction of the adhesive layer before curing is α (%) and the gel fraction of the cured layer obtained by curing the adhesive layer is β (%), and the increase rate (%) of the gel fraction, expressed by the formula: [(β-α) / α]×100, is 60% or more.
3. A thermosetting adhesive sheet according to claim 1 or 2, wherein the cured layer obtained by heat-treating the adhesive layer at 170°C for 2 hours has a tensile modulus of elasticity at 25°C of 0.5 GPa or more.
4. The thermosetting adhesive sheet according to claim 1 or 2, which satisfies the formula: Y / X<1, where X (μm) is the thickness of the adhesive layer and Y (μm) is the average particle size of the (C) component.
5. The thermosetting adhesive sheet according to claim 1 or 2, wherein the component (C) is an inorganic filler that has not been surface-treated.
6. The thermosetting adhesive sheet according to claim 1 or 2, wherein the component (C) is a spherical filler.
7. The thermosetting adhesive sheet according to claim 1 or 2, wherein the adhesive layer further contains a thermal polymerization initiator as component (D).
8. The thermosetting adhesive sheet according to claim 1 or 2, which is used for forming an insulating layer of a device.
9. A laminate comprising a conductive layer and an insulating layer formed on the conductive layer, wherein the insulating layer is a layer formed by curing the adhesive layer of the thermosetting adhesive sheet according to claim 1 or 2.
10. A method for producing a laminate according to claim 9, comprising: a step (I) of obtaining a laminate by laminating a thermosetting adhesive sheet according to claim 1 or 2 onto a conductive layer; and a step (II) of heating the laminate to a predetermined temperature to cure the adhesive layer of the thermosetting adhesive sheet.
11. A method for producing a laminate according to claim 10, comprising, after step (I) and before step (II), a step (I-1) of forming an insulating resin layer on the thermosetting adhesive sheet according to claim 1 or 2.
Citation Information
Patent Citations
Thermosetting adhesive composition and laminated film
JP2021025016A
Modified hydrogenated polyolefin, resin composition, insulating film, semiconductor device, and method for producing modified hydrogenated polyolefin
JP2021054889A
Adhesive composition, thermosetting adhesive sheet, and printed wiring board
WO2019151014A1
Curable adhesive composition and curable adhesive sheet
WO2023002970A1