Solid polymer electrolyte membrane, membrane electrode assembly, water electrolysis device, and method for manufacturing solid polymer electrolyte membrane
The solid polymer electrolyte membrane, featuring a fluorine-containing polymer and polyphenylene sulfide fibers, addresses the issues of strength and resistance in water electrolysis devices, enhancing the efficiency of power-to-gas conversion and storage by providing improved surface quality and reduced membrane resistance.
Patent Information
- Application Number
- PCT/JP2024/011665
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-03
AI Technical Summary
Existing solid polymer electrolyte membranes for water electrolysis devices lack sufficient strength, surface quality, and low membrane resistance, which are essential for efficient power-to-gas conversion and storage applications.
A solid polymer electrolyte membrane comprising a fluorine-containing polymer with an ion exchange group and a nonwoven fabric containing polyphenylene sulfide fibers, with a specific fiber diameter distribution and content, is used to enhance strength and surface properties while reducing membrane resistance.
The proposed membrane achieves excellent strength and surface quality, along with low membrane resistance, making it suitable for water electrolysis devices, thereby improving the efficiency of power-to-gas conversion and storage.
Smart Images

Figure JP2024011665_03102024_PF_FP_ABST
Abstract
Description
Solid polymer electrolyte membrane, membrane electrode assembly, water electrolysis device, and method for manufacturing solid polymer electrolyte membrane
[0001] The present invention relates to a solid polymer electrolyte membrane, a membrane electrode assembly, a water electrolysis device, and a method for producing a solid polymer electrolyte membrane.
[0002] From the viewpoint of power-to-gas, i.e., converting surplus electricity into gas for storage and utilization, the use of a polymer electrolyte membrane (PEM water electrolysis device) has been considered. For example, Patent Document 1 discloses a water electrolysis device including a solid polymer electrolyte membrane containing a fluoropolymer having ion exchange groups and a woven fabric.
[0003] International Publication No. 2019 / 088299
[0004] In a water electrolysis device, which is one application of a solid polymer electrolyte membrane, the solid polymer electrolyte membrane that separates an anode chamber and a cathode chamber is subjected to high pressure. Therefore, the solid polymer electrolyte membrane is required to have excellent strength. Furthermore, in a water electrolysis device including a solid polymer electrolyte membrane, it is preferable that the membrane resistance be as low as possible. Furthermore, in a solid polymer electrolyte membrane, it is preferable that only a polymer having an ion exchange group is observed on its surface. For example, when a solid polymer electrolyte membrane includes a reinforcing material, it is preferable that the reinforcing material is not observed on the surface. Hereinafter, when only a polymer is observed on the surface of a solid polymer electrolyte membrane and no reinforcing material is observed, this is referred to as having excellent surface properties. The present inventors evaluated a solid polymer electrolyte membrane as described in Patent Document 1 and a water electrolysis device including the electrolyte membrane and found that the above three problems were not resolved and further improvements are necessary.
[0005] The present invention has been made in view of the above problems, and an object of the present invention is to provide a solid polymer electrolyte membrane that is excellent in strength and surface properties and that can reduce membrane resistance when applied to a water electrolysis device. Another object of the present invention is to provide a membrane electrode assembly, a water electrolysis device, and a method for manufacturing the solid polymer electrolyte membrane.
[0006] As a result of extensive research into the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by the following configuration.
[0007] (1) A solid polymer electrolyte membrane comprising a fluoropolymer having an ion exchange group and a nonwoven fabric, wherein the nonwoven fabric contains polyphenylene sulfide fibers, a fiber diameter distribution histogram of the fibers constituting the nonwoven fabric has a maximum frequency peak in the range of 100 to 900 nm, and the thickness of the solid polymer electrolyte membrane is 30 to 90 μm. (2) The solid polymer electrolyte membrane according to (1), wherein the ion exchange group of the fluoropolymer is a sulfonic acid type functional group. (3) The solid polymer electrolyte membrane according to (1) or (2), wherein the fluoropolymer contains at least one unit selected from the group consisting of a unit represented by formula (1-1) described below, a unit represented by formula (1-2) described below, a unit represented by formula (1-3) described below, and a unit represented by formula (1-4) described below. (4) The solid polymer electrolyte membrane according to any of (1) to (3), comprising at least one element selected from the group consisting of platinum, palladium, cerium, and manganese. (5) The solid polymer electrolyte membrane according to any one of (1) to (4), wherein the content of the nonwoven fabric is 5% by mass or more and 40% by mass or less, based on the total mass of the solid polymer electrolyte membrane. (6) The solid polymer electrolyte membrane according to any one of (1) to (5), which is used for water electrolysis. (7) A membrane electrode assembly comprising the solid polymer electrolyte membrane according to any one of (1) to (6), a cathode catalyst layer disposed on one side of the solid polymer electrolyte membrane, and an anode catalyst layer disposed on the other side of the solid polymer electrolyte membrane. (8) A water electrolysis device comprising the membrane electrode assembly according to (7), a power supply unit connected to the cathode catalyst layer side and the anode catalyst layer side of the membrane electrode assembly, and a water supply unit that supplies water to the anode catalyst layer side. (9) A method for producing the solid polymer electrolyte membrane according to any one of (1) to (6), comprising: Step 1 of converting groups convertible to ion-exchange groups in a precursor membrane comprising a polymer having groups convertible to ion-exchange groups and a nonwoven fabric into ion-exchange groups; and Step 2 of drying the membrane obtained in Step 1 while restraining its periphery to obtain a solid polymer electrolyte membrane.(10) The method for producing a solid polymer electrolyte membrane according to (9), further comprising a step 3 of obtaining a precursor membrane by sandwiching a nonwoven fabric between a plurality of polymer membranes containing a polymer having a group that can be converted into an ion-exchange group, before step 1. (11) The method for producing a solid polymer electrolyte membrane according to (10), further comprising a step 4 of kneading a compound containing at least one element selected from the group consisting of platinum, palladium, cerium, and manganese with a polymer having a group that can be converted into an ion-exchange group, and extruding the resulting kneaded mixture to obtain a precursor membrane, before step 3.
[0008] According to the present invention, it is possible to provide a solid polymer electrolyte membrane that is excellent in strength and surface properties and that can reduce membrane resistance when applied to a water electrolysis device. Furthermore, according to the present invention, it is possible to provide a membrane electrode assembly, a water electrolysis device, and a method for producing a solid polymer electrolyte membrane.
[0009] 1 is a cross-sectional view schematically illustrating an example of a membrane electrode assembly of the present invention.
[0010] The definitions of the following terms apply throughout the present specification and claims unless otherwise specified. An "ion exchange group" is a group that can exchange at least a portion of the ions contained in this group with other ions, and examples thereof include the sulfonic acid functional group and carboxylic acid functional group shown below. A "sulfonic acid functional group" is a sulfonic acid group (-SO 3 Here, the form of the sulfonate group is, for example, (—SO 3 - ) Ma + , (-SO 3 - ) 2 Mb 2+ , and (-SO 3 - ) 3 Mc 3+ (However, Ma + is an alkali metal ion or a quaternary ammonium cation, and Mb 2+ is a divalent metal ion, Mc 3+is a trivalent metal ion.) When there are two ligands, the number of ion exchange groups is counted as two, and when there are three ligands, the number of ion exchange groups is counted as three. "Carboxylic acid type functional group" means a carboxylic acid group (-COOH) or a carboxylic acid salt group. Here, the form of the carboxylic acid salt group can be, for example, (-COO - ) Ma + , (-COO - ) 2 Mb 2+ , and (-COO - ) 3 Mc 3+ (However, Ma + is an alkali metal ion or a quaternary ammonium cation, and Mb 2+ is a divalent metal ion, Mc 3+ is a trivalent metal ion.) Note that when there are two ligands, the number of ion exchange groups is counted as two, and when there are three ligands, the number of ion exchange groups is counted as three. A "precursor membrane" is a membrane containing a polymer having a group that can be converted into an ion exchange group. A "group that can be converted into an ion exchange group" means a group that can be converted into an ion exchange group by treatment such as hydrolysis or acidification. A "group that can be converted into a sulfonic acid functional group" means a group that can be converted into a sulfonic acid functional group by treatment such as hydrolysis or acidification. A "group that can be converted into a carboxylic acid functional group" means a group that can be converted into a carboxylic acid functional group by known treatment such as hydrolysis or acidification.
[0011] The term "unit" in a polymer refers to an atomic group derived from one molecule of a monomer formed by polymerization of the monomer. The unit may be an atomic group formed directly by the polymerization reaction, or may be an atomic group in which a part of the atomic group is converted into a different structure by treating the polymer obtained by the polymerization reaction.
[0012] A numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the upper and lower limits. In the numerical ranges described in stages in this specification, the upper or lower limit described in a certain numerical range may be replaced with the upper or lower limit of another numerical range described in stages. Furthermore, in the numerical ranges described in this specification, the upper or lower limit described in a certain numerical range may be replaced with a value shown in the examples.
[0013] [Electrolyte Membrane] The solid polymer electrolyte membrane of the present invention (hereinafter also simply referred to as "electrolyte membrane") is a solid polymer electrolyte membrane comprising a fluoropolymer having ion exchange groups (hereinafter also simply referred to as "fluoropolymer (I)") and a nonwoven fabric, wherein the nonwoven fabric comprises polyphenylene sulfide fibers, and a fiber diameter distribution histogram of the fibers constituting the nonwoven fabric has a maximum frequency peak in the range of 100 to 900 nm, and the thickness of the solid polymer electrolyte membrane is 30 to 90 μm. As described above, the electrolyte membrane has excellent strength and surface properties, and can reduce membrane resistance when applied to a water electrolysis device. The above effects are obtained, first, because the electrolyte membrane uses a nonwoven fabric containing fibers with a small fiber diameter, which results in excellent surface properties. Note that, as shown in Comparative Example 1 described below, when the electrolyte membrane comprises a woven fabric, the overlapping portions of the warp fibers and weft fibers are likely to be exposed on the surface, resulting in poor surface properties. Furthermore, since the fiber diameter of the fibers contained in the nonwoven fabric is within the predetermined range, the membrane resistance tends to be low when the electrolyte membrane is applied to a water electrolysis device. Furthermore, since the nonwoven fabric contains polyphenylene sulfide fibers, the strength of the electrolyte membrane is excellent.
[0014] The electrolyte membrane may have a single layer structure or a multilayer structure. A specific example of an electrolyte membrane having a multilayer structure is a structure in which a plurality of electrolyte membranes having different ion exchange capacities are stacked.
[0015] The thickness of the electrolyte membrane is 30 to 90 μm, preferably 40 to 90 μm, and more preferably 50 to 90 μm, from the viewpoint of high mechanical strength and low cell resistance. When the electrolyte membrane has a multilayer structure, the thickness of the electrolyte membrane refers to the total thickness of each layer. The thickness of the electrolyte membrane is measured using a magnified image (objective lens magnification: 50x) of the cross section of the electrolyte membrane photographed using a laser microscope (product name "VK-X1000", manufactured by Keyence Corporation) under conditions of a temperature of 25°C and a relative humidity of 50% RH.
[0016] Each of the components included in the solid polymer electrolyte membrane will be described in detail below.
[0017] <Nonwoven Fabric> The nonwoven fabric serves to improve the dimensional stability, strength, handleability, etc. of the electrolyte membrane. The nonwoven fabric contains polyphenylene sulfide fibers. The nonwoven fabric may be made of polyphenylene sulfide fibers alone, or may be made of polyphenylene sulfide fibers and fibers other than polyphenylene sulfide fibers. In particular, the nonwoven fabric is preferably made of polyphenylene sulfide fibers alone.
[0018] In a fiber diameter distribution histogram of the fibers constituting the nonwoven fabric, the maximum frequency peak is in the range of 100 to 900 nm. The maximum frequency peak is preferably in the range of 350 to 850 nm, and more preferably in the range of 600 to 800 nm. The maximum frequency peak can be derived by creating a histogram of the frequency of the number of fibers constituting the nonwoven fabric and the fiber diameter distribution. First, the fiber diameter and number of fibers are measured to create the histogram. The entire nonwoven fabric is observed with a scanning electron microscope (magnification 20,000x) and derived from the resulting two-dimensional image. The number of fibers is counted as one fiber, with each continuous fiber counted within the obtained two-dimensional image. The fiber diameter is measured as the length in the direction perpendicular to the longitudinal direction of the fiber in the obtained two-dimensional image. This measurement is repeated by changing the position of the scanning electron microscope observation until 100 or more fiber diameters have been measured. A histogram of the fiber diameter distribution is created from the distribution of the number of fibers for each fiber diameter obtained above. To create the histogram, the X-axis represents the fiber diameter (nm) and the Y-axis represents the frequency. The histogram is created with a class width of 20 nm. For example, if the maximum fiber diameter is 2000 nm and the minimum fiber diameter is 20 nm, and the class width of the histogram is 20 nm, the number of bins (number of fibers in the histogram) is (2000 - 20) ÷ 20 = 99 (fibers). The maximum frequency peak in the fiber diameter distribution histogram refers to the class (interval) with the highest frequency in the fiber diameter distribution histogram. The fiber diameter corresponding to the maximum frequency peak is the lower limit fiber diameter of the class with the highest frequency. For example, if the class with the highest frequency is 100 nm or more and less than 120 nm, the fiber diameter at the maximum frequency peak is 100 nm.
[0019] The basis weight of the nonwoven fabric is 1 to 50 g / m2 in terms of high mechanical strength and low cell resistance. 2 is preferred, and 3 to 30 g / m 2 The basis weight of the nonwoven fabric is determined by cutting the nonwoven fabric into a piece of 0.15 m long and 0.15 m wide, measuring the mass using a precision electronic balance, and 2 This is the value converted to mass per unit.
[0020] The thickness of the nonwoven fabric is preferably 5 to 70 μm, more preferably 5 to 50 μm, and even more preferably 15 to 40 μm, from the viewpoints of high mechanical strength and low cell resistance. The thickness of the nonwoven fabric is measured by placing the nonwoven fabric on a dial gauge stand 7002 (Mitsutoyo) and using a digital gauge 543-250 (Mitsutoyo) with a flat terminal with a diameter of 5 mm attached to the tip.
[0021] The method for producing a nonwoven fabric is not particularly limited, but examples include a method for producing a wet-laid nonwoven fabric by producing islands-in-sea composite fibers and then dissolving and removing the sea component to produce nanofiber fibers, as disclosed in JP 2019-197702 A; a method for producing a nonwoven fabric using an electrospinning method, as disclosed in JP 2017-197876 A; and a method for producing a nonwoven fabric using a known melt-blowing method, as disclosed in JP 2-80651 A.
[0022] The content of the nonwoven fabric is preferably 3 mass % or more, more preferably 5 mass % or more, and is preferably 50 mass % or less, more preferably 40 mass % or less, and even more preferably 30 mass % or less, based on the total mass of the electrolyte membrane.
[0023] <Fluoropolymer (I)> The ion exchange capacity of the fluoropolymer (I) is preferably 0.90 milliequivalents / gram dry resin or more, more preferably greater than 1.10 milliequivalents / gram dry resin, even more preferably 1.15 milliequivalents / gram dry resin or more, particularly preferably 1.20 milliequivalents / gram dry resin or more, and most preferably 1.25 milliequivalents / gram dry resin or more, from the viewpoint of the strength of the membrane / electrode assembly when water is contained. The ion exchange capacity of the fluoropolymer (I) is preferably 2.00 milliequivalents / gram dry resin or less, more preferably 1.50 milliequivalents / gram dry resin or less, and even more preferably 1.43 milliequivalents / gram dry resin or less, from the viewpoint of the strength of the membrane / electrode assembly when water is contained. Only one type of fluoropolymer (I) may be used, or two or more types may be used in a laminated or mixed state.
[0024] The electrolyte membrane may contain a polymer other than the fluorine-containing polymer (I), but it is preferable that the polymer in the electrolyte membrane essentially consists of the fluorine-containing polymer (I). "Essentially consisting of the fluorine-containing polymer (I)" means that the content of the fluorine-containing polymer (I) is 95% by mass or more relative to the total mass of the polymers in the electrolyte membrane. The upper limit of the content of the fluorine-containing polymer (I) can be 100% by mass relative to the total mass of the polymers in the electrolyte membrane. Specific examples of other polymers than the fluorine-containing polymer (I) include one or more polyazole compounds selected from the group consisting of polymers of heterocyclic compounds containing one or more nitrogen atoms in the ring, and polymers of heterocyclic compounds containing one or more nitrogen atoms and oxygen atoms and / or sulfur atoms in the ring. Specific examples of the polyazole compound include polyimidazole compounds, polybenzimidazole compounds, polybenzobisimidazole compounds, polybenzoxazole compounds, polyoxazole compounds, polythiazole compounds, and polybenzothiazole compounds. In view of the oxidation resistance of the electrolyte membrane, other polymers include polyphenylene sulfide resin and polyphenylene ether resin.
[0025] The fluoropolymer (I) has an ion-exchange group. Specific examples of the ion-exchange group include a sulfonic acid type functional group and a carboxylic acid type functional group, and the sulfonic acid type functional group is preferred from the viewpoint of further reducing the electrolysis voltage when the electrolyte membrane is applied to a water electrolysis device. Below, mainly, embodiments of the fluoropolymer having a sulfonic acid type functional group (hereinafter, also referred to as "fluoropolymer (S)") will be described in detail.
[0026] The fluorine-containing polymer (S) preferably contains a unit based on a fluorine-containing olefin and a unit having a sulfonic acid functional group and a fluorine atom. Examples of the fluorine-containing olefin include fluoroolefins having 2 to 3 carbon atoms and having one or more fluorine atoms in the molecule. Specific examples of the fluoroolefin include tetrafluoroethylene (hereinafter also referred to as "TFE"), chlorotrifluoroethylene, vinylidene fluoride, vinyl fluoride, and hexafluoropropylene. Among these, TFE is preferred from the viewpoints of the production cost of the monomer, reactivity with other monomers, and excellent properties of the resulting fluorine-containing polymer (S). One type of fluorine-containing olefin may be used alone, or two or more types may be used in combination.
[0027] As the unit having a sulfonic acid type functional group and a fluorine atom, a unit represented by formula (1) is preferred. 2 -CF(-L-(SO 3 M) n )]-
[0028] L is an (n+1)-valent perfluorohydrocarbon group which may contain an etheric oxygen atom. The etheric oxygen atom may be located at a terminal of the perfluorohydrocarbon group or between carbon atoms. The (n+1)-valent perfluorohydrocarbon group preferably has 1 or more carbon atoms, more preferably 2 or more carbon atoms, and preferably 20 or less, more preferably 10 or less.
[0029] L is preferably an (n+1)-valent perfluoroaliphatic hydrocarbon group which may contain an etheric oxygen atom, more preferably a divalent perfluoroalkylene group which may contain an etheric oxygen atom, where n = 1, or a trivalent perfluoroaliphatic hydrocarbon group which may contain an etheric oxygen atom, where n = 2. The divalent perfluoroalkylene group may be either linear or branched.
[0030] M is a hydrogen atom, an alkali metal, or a quaternary ammonium cation, and n is 1 or 2.
[0031] The unit represented by formula (1) is preferably a unit represented by formula (1-1), a unit represented by formula (1-2), a unit represented by formula (1-3), or a unit represented by formula (1-4). 2 -CF(-O-R f1 -SO 3 M)] - Formula (1-2) - [CF 2 -CF(-R f1 -SO 3 M) ]-
[0032]
[0033]
[0034] R f1 is a perfluoroalkylene group which may contain an oxygen atom between carbon atoms. The number of carbon atoms in the perfluoroalkylene group is preferably 1 or more, more preferably 2 or more, and is preferably 20 or less, more preferably 10 or less.
[0035] R f2 is a single bond or a perfluoroalkylene group which may contain an oxygen atom between carbon atoms. The number of carbon atoms in the perfluoroalkylene group is preferably 1 or more, more preferably 2 or more, and is preferably 20 or less, more preferably 10 or less.
[0036] R f3 is a single bond or a perfluoroalkylene group which may contain an oxygen atom between carbon atoms. The number of carbon atoms in the perfluoroalkylene group is preferably 1 or more, more preferably 2 or more, and is preferably 20 or less, more preferably 10 or less.
[0037] r is 0 or 1. m is 0 or 1. M is a hydrogen atom, an alkali metal, or a quaternary ammonium cation.
[0038] As the unit represented by formula (1-1) and the unit represented by formula (1-2), a unit represented by formula (1-5) is more preferred. 2 -CF(-(CF 2 ) x -(OCF 2 CFY) y-O-(CF 2 ) z -SO 3 M)]—x is 0 or 1, y is an integer from 0 to 2, z is an integer from 1 to 4, and Y is F or CF 3 M is as described above.
[0039] Specific examples of the unit represented by formula (1-1) include the following units. In the formula, w is an integer of 1 to 8, and x is an integer of 1 to 5. The definition of M in the formula is as described above. -[CF 2 -CF(-O-(CF 2 ) w -SO 3 M)]- -[CF 2 -CF(-O-CF 2 CF (CF 3 )-O-(CF 2 ) w -SO 3 M)]- -[CF 2 -CF(-(O-CF 2 CF (CF 3 )) x -SO 3 M) ]-
[0040] Specific examples of the unit represented by formula (1-2) include the following units. In the formula, w is an integer of 1 to 8. The definition of M in the formula is as described above. -[CF 2 -CF(-(CF 2 ) w -SO 3 M)]- -[CF 2 -CF (-CF 2 -O-(CF 2 ) w -SO 3 M) ]-
[0041] The unit represented by formula (1-3) is preferably a unit represented by formula (1-3-1), where M is defined as above.
[0042]
[0043] R f4 is a linear perfluoroalkylene group having 1 to 6 carbon atoms, and R f5is a single bond or a linear perfluoroalkylene group having 1 to 6 carbon atoms which may contain an oxygen atom between the carbon atoms. The definitions of r and M are as described above.
[0044] Specific examples of the unit represented by formula (1-3-1) include the following.
[0045]
[0046] As the unit represented by formula (1-4), a unit represented by formula (1-4-1) is preferred. f1 , R f2 and M are defined as above.
[0047]
[0048] Specific examples of the unit represented by formula (1-4-1) include the following.
[0049]
[0050] The unit having a sulfonic acid type functional group and a fluorine atom may be used alone or in combination of two or more.
[0051] The fluoropolymer (I) may contain units based on other monomers other than the units based on fluorine-containing olefins and the units having a sulfonic acid functional group and a fluorine atom. Specific examples of other monomers include CF 2 = CFR f6 (However, R f6 is a perfluoroalkyl group having 2 to 10 carbon atoms, CF 2 =CF-OR f7 (However, R f7 is a perfluoroalkyl group having 1 to 10 carbon atoms, CF 2 = CFO (CF 2 ) v CF = CF 2 (wherein v is an integer of 1 to 3.) The content of units based on other monomers is preferably at most 30 mass % based on all units in the fluoropolymer (I) from the viewpoint of maintaining ion exchange performance.
[0052] The content of the fluoropolymer (I) is preferably from 95 to 100% by mass based on the total mass of the electrolyte membrane.
[0053] <Other Components> The electrolyte membrane preferably contains at least one element selected from the group consisting of platinum, palladium, cerium, and manganese. These elements may be present in the electrolyte membrane in the form of metal itself, oxide, alloy, ion, salt, or the like.
[0054] Platinum may exist in the electrolyte membrane as platinum itself, platinum oxide, platinum-containing composite metal oxide, or platinum alloy. In other words, the electrolyte membrane may contain a platinum-containing material. Specific examples of platinum-containing composite oxides include M x Pt 3 O 4 (M is at least one metal atom selected from the group consisting of Li, Na, Mg, Ca, Zn, Cd, Co, Ni, Mn, Cu, Ag, Bi, and Ce, and x is greater than 0 and equal to or less than 1.) Specific examples of platinum alloys include alloys containing platinum and at least one metal selected from the group consisting of transition metals and noble metals other than platinum.
[0055] Specific examples of the shape of the platinum-containing material include particles and sheets. When the platinum-containing material is in the form of particles, the platinum-containing material may be core-shell type particles. An example of a core-shell type particle is a particle in which the core is carbon or contains a metal other than platinum, and the shell contains platinum atoms.
[0056] The platinum-containing material may be supported on a carrier. Specific examples of the carrier include carbon carriers such as carbon black powder, graphitized carbon, carbon fiber, and carbon nanotubes. When the platinum-containing material is supported on a carrier, the amount of the platinum-containing material supported is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, and preferably 50% by mass or less, based on the total mass of the platinum-containing material and the carrier.
[0057] Palladium may be present in the electrolyte membrane as palladium itself, palladium oxide, a composite metal oxide containing palladium, or a palladium alloy. In other words, the electrolyte membrane may contain a palladium-containing substance.
[0058] Cerium and manganese decompose hydrogen peroxide, hydroxyl radicals, and hydroperoxyl radicals, which are substances that cause deterioration of the solid polymer electrolyte membrane. Cerium and manganese are preferably present in the solid polymer electrolyte membrane as ions, and may be present in any state in the solid polymer electrolyte membrane as long as they are present as ions.
[0059] <Method for Producing Electrolyte Membrane> One example of a method for producing an electrolyte membrane is the following method (Method 1). First, a polymer (hereinafter also referred to as "fluoropolymer (I')") of a fluoromonomer having a group convertible to an ion-exchange group (hereinafter also referred to as fluoromonomer (I')) is prepared by converting the group convertible to an ion-exchange group into an ion-exchange group to obtain a fluoropolymer (I). Next, a dispersion of the fluoropolymer (I) is impregnated into a nonwoven fabric, followed by drying to obtain an electrolyte membrane containing the fluoropolymer (I) and the nonwoven fabric.
[0060] Another example of the method for producing an electrolyte membrane is the following method (Method 2). First, a composition containing the fluoropolymer (I) is used to obtain a membrane P1 containing the fluoropolymer (I). Next, the membrane P1, nonwoven fabric, and membrane P1 are arranged in this order, and these are laminated using a laminating roll or a vacuum laminating device to obtain an electrolyte membrane containing the fluoropolymer (I) and the nonwoven fabric.
[0061] Another example of a method for producing an electrolyte membrane is the following method (Method 3). First, a composition containing the fluoropolymer (I') is used to obtain a membrane P2 containing the fluoropolymer (I'). Next, the membrane P2, nonwoven fabric, and membrane P2 are arranged in this order, and these are laminated using a laminating roll or a vacuum laminating device to obtain a precursor membrane containing the fluoropolymer (I') and the nonwoven fabric. Next, a method is given in which groups in the fluoropolymer (I') in the obtained precursor membrane that can be converted into ion-exchange groups are converted into ion-exchange groups to obtain an electrolyte membrane containing the fluoropolymer (I) and the nonwoven fabric.
[0062] In order to produce an electrolyte membrane containing at least one element selected from the group consisting of platinum, palladium, cerium, and manganese, for example, in the case of the above-mentioned Method 1, a method in which at least one element selected from the group consisting of platinum, palladium, cerium, and manganese is contained in a dispersion in which the fluoropolymer (I) is dispersed can be mentioned. In the case of the above-mentioned Method 2, a method in which at least one element selected from the group consisting of platinum, palladium, cerium, and manganese is contained in a composition containing the fluoropolymer (I). Furthermore, in the case of the above-mentioned Method 3, a method in which at least one element selected from the group consisting of platinum, palladium, cerium, and manganese is contained in a composition containing the fluoropolymer (I') can be mentioned.
[0063] The fluoropolymer (I') is preferably a polymer (hereinafter also referred to as "fluoropolymer (S')") of a fluoromonomer having a group that can be converted into a sulfonic acid type functional group (hereinafter also referred to as "fluoromonomer (S')"), and particularly preferably a copolymer of a fluorine-containing olefin and a monomer having a group that can be converted into a sulfonic acid type functional group and a fluorine atom. The fluoropolymer (S') will be described in detail below.
[0064] As the method for copolymerizing the fluoropolymer (S'), known methods such as solution polymerization, suspension polymerization and emulsion polymerization can be adopted.
[0065] Examples of the fluorine-containing olefin include those exemplified above, and TFE is preferred from the viewpoints of the production cost of the monomer, the reactivity with other monomers, and the excellent properties of the resulting fluorine-containing polymer (S). One type of fluorine-containing olefin may be used alone, or two or more types may be used in combination.
[0066] The fluorine-containing monomer (S') may be a compound having one or more fluorine atoms in the molecule, an ethylenic double bond, and a group that can be converted into a sulfonic acid functional group. As the fluorine-containing monomer (S'), a compound represented by formula (2) is preferred in terms of the production cost of the monomer, reactivity with other monomers, and excellent properties of the resulting fluorine-containing polymer (S). Formula (2) CF 2 =CF-L-(A) n The definitions of L and n in formula (2) are as described above. A is a group that can be converted into a sulfonic acid functional group. The group that can be converted into a sulfonic acid functional group is preferably a functional group that can be converted into a sulfonic acid functional group by hydrolysis. Specific examples of groups that can be converted into a sulfonic acid functional group include -SO 2 F, -SO 2 Cl, —SO 2 Br is an example.
[0067] The compound represented by formula (2) is preferably a compound represented by formula (2-1), a compound represented by formula (2-2), a compound represented by formula (2-3), or a compound represented by formula (2-4). 2 =CF-O-R f1 -A Formula (2-2) CF 2 =CF-R f1 -A
[0068]
[0069] R in the formula f1 , R f2 , r and A are as defined above.
[0070]
[0071] R in the formula f1 , R f2 , R f3, r, m and A are as defined above.
[0072] The compound represented by formula (2-1) and the compound represented by formula (2-1) are preferably compounds represented by formula (2-5): Formula (2-5) CF 2 =CF-(CF 2 ) x -(OCF 2 CFY) y -O-(CF 2 ) z -SO 3 The definitions of x, y, z and Y in the formula F are as described above.
[0073] Specific examples of the compound represented by formula (2-1) include the following compounds. In the formula, w is an integer of 1 to 8, and x is an integer of 1 to 5. CF 2 =CF-O-(CF 2 ) w -SO 2 FCF 2 =CF-O-CF 2 CF (CF 3 )-O-(CF 2 ) w -SO 2 FCF 2 =CF-[O-CF 2 CF (CF 3 )] x -SO 2 F
[0074] Specific examples of the compound represented by formula (2-2) include the following compounds: In the formula, w is an integer of 1 to 8. CF 2 =CF-(CF 2 ) w -SO 2 FCF 2 =CF-CF 2 -O-(CF 2 ) w -SO 2 F
[0075] The compound represented by formula (2-3) is preferably a compound represented by formula (2-3-1).
[0076]
[0077] R in the formula f4 , R f5 , r and A are as defined above.
[0078] Specific examples of the compound represented by formula (2-3-1) include the following.
[0079]
[0080] The compound represented by formula (2-4) is preferably a compound represented by formula (2-4-1).
[0081]
[0082] R in the formula f1 , R f2 and A are defined as above.
[0083] Specific examples of the compound represented by formula (2-4-1) include the following.
[0084]
[0085] The fluorine-containing monomer (S') may be used alone or in combination of two or more. In the production of the fluorine-containing polymer (S'), in addition to the fluorine-containing olefin and the fluorine-containing monomer (S'), other monomers may be further used. Examples of other monomers include those exemplified above.
[0086] The ion exchange capacity of the fluoropolymer (I') can be adjusted by changing the content of groups that can be converted into ion exchange groups in the fluoropolymer (I').
[0087] Specific examples of methods for converting groups convertible to ion-exchange groups into ion-exchange groups include methods of subjecting the precursor membrane to hydrolysis treatment, acidification treatment, etc. Among these, a method of contacting the precursor membrane with an alkaline aqueous solution is preferred.
[0088] Specific examples of the method for contacting the precursor film with the alkaline aqueous solution include immersing the precursor film in the alkaline aqueous solution and spraying the alkaline aqueous solution onto the surface of the precursor film. The temperature of the alkaline aqueous solution is preferably 30° C. or higher, more preferably 40° C. or higher, and preferably 100° C. or lower. The contact time between the precursor film and the alkaline aqueous solution is preferably 3 minutes or longer, more preferably 5 minutes or longer, and preferably 150 minutes or shorter, more preferably 50 minutes or shorter.
[0089] The alkaline aqueous solution preferably contains an alkali metal hydroxide, a water-soluble organic solvent, and water. Examples of alkali metal hydroxides include sodium hydroxide and potassium hydroxide. In this specification, the water-soluble organic solvent refers to an organic solvent that is easily soluble in water. Specifically, an organic solvent having a solubility of 0.1 g or more in 1000 ml of water (20°C) is preferred, and an organic solvent having a solubility of 0.5 g or more is particularly preferred. The water-soluble organic solvent preferably contains at least one selected from the group consisting of aprotic organic solvents, alcohols, and aminoalcohols, and particularly preferably contains an aprotic organic solvent. One water-soluble organic solvent may be used alone, or two or more may be used in combination.
[0090] Specific examples of aprotic organic solvents include dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, and N-ethyl-2-pyrrolidone, with dimethyl sulfoxide being preferred. Specific examples of alcohols include methanol, ethanol, isopropanol, butanol, methoxyethoxyethanol, butoxyethanol, butylcarbitol, hexyloxyethanol, octanol, 1-methoxy-2-propanol, and ethylene glycol. Specific examples of aminoalcohols include ethanolamine, N-methylethanolamine, N-ethylethanolamine, 1-amino-2-propanol, 1-amino-3-propanol, 2-aminoethoxyethanol, 2-aminothioethoxyethanol, and 2-amino-2-methyl-1-propanol.
[0091] The concentration of the alkali metal hydroxide in the alkaline aqueous solution is preferably 1% by mass or more, more preferably 3% by mass or more, and preferably 60% by mass or less, more preferably 55% by mass or less. The content of the water-soluble organic solvent in the alkaline aqueous solution is preferably 1% by mass or more, more preferably 3% by mass or more, and preferably 60% by mass or less, more preferably 55% by mass or less. The concentration of water in the alkaline aqueous solution is preferably 39 to 80% by mass.
[0092] After the precursor film is brought into contact with the alkaline aqueous solution, a treatment for removing the alkaline aqueous solution may be carried out. As a method for removing the alkaline aqueous solution, for example, a method for washing the precursor film that has been brought into contact with the alkaline aqueous solution with water may be mentioned.
[0093] After contacting the precursor membrane with the alkaline aqueous solution, the resulting membrane may be contacted with an acidic aqueous solution to convert the ion exchange groups to an acid form. Specific examples of methods for contacting the precursor membrane with the acidic aqueous solution include immersing the precursor membrane in the acidic aqueous solution and spraying the acidic aqueous solution onto the surface of the precursor membrane. The acidic aqueous solution preferably contains an acid component and water. Specific examples of the acid component include hydrochloric acid and sulfuric acid.
[0094] One preferred embodiment of the method for producing a solid polymer electrolyte of the present invention includes a step 1 of converting groups convertible to ion-exchange groups in a precursor membrane containing a polymer and a nonwoven fabric having groups convertible to ion-exchange groups into ion-exchange groups, and a step 2 of drying the membrane obtained in step 1 while restraining the periphery to obtain a solid polymer electrolyte membrane. Specific procedures for step 1 include the above-mentioned method of subjecting the precursor membrane to a hydrolysis treatment or an acid-form treatment. Specific procedures for step 2 include, for example, a method of drying the membrane obtained in step 1 at a temperature equal to or higher than the softening point of the polymer while fixing the periphery of the membrane with a metal restraining frame.
[0095] The method may further include, before step 1, step 3 of sandwiching the nonwoven fabric between a plurality of polymer films containing a polymer having a group that can be converted into an ion-exchange group to obtain a precursor membrane.The method may further include, before step 3, step 4 of kneading a compound containing at least one element selected from the group consisting of platinum, palladium, cerium, and manganese with a polymer having a group that can be converted into an ion-exchange group, and extruding the resulting kneaded mixture to obtain a precursor membrane.
[0096] [Membrane Electrode Assembly] The membrane electrode assembly of the present invention includes the above-mentioned electrolyte membrane, a cathode catalyst layer disposed on one side of the electrolyte membrane, and an anode catalyst layer disposed on the other side of the electrolyte membrane.
[0097] 1 is a cross-sectional view schematically illustrating an example of a membrane electrode assembly of the present invention, showing a case where the electrolyte membrane has a single-layer structure. In the example of Fig. 1, the membrane electrode assembly 20 includes an anode 22 having a catalyst layer 26 and a gas diffusion layer 28, a cathode 24 having the catalyst layer 26 and the gas diffusion layer 28, and an electrolyte membrane 10 disposed between the anode 22 and the cathode 24 in contact with the catalyst layer 26.
[0098] In the example of FIG. 1, the electrolyte membrane has a single layer structure, but the electrolyte membrane may have a multi-layer structure.
[0099] <Anode and Cathode> The anode and cathode each have a catalyst layer. In the example of Figure 1, the anode 22 and cathode 24 each have a catalyst layer 26 and a gas diffusion layer 28.
[0100] Specific examples of the catalyst layer include a layer containing a catalyst and a polymer having an ion exchange group.Specific examples of the catalyst include a supported catalyst in which a catalyst containing platinum, a platinum alloy, or a platinum having a core-shell structure is supported on a carbon support, an iridium oxide catalyst, a composite oxide catalyst containing iridium and other metal elements, an alloy containing iridium oxide, and a catalyst containing iridium oxide having a core-shell structure.An example of the carbon support is carbon black powder.An example of the polymer having an ion exchange group is a fluorine-containing polymer having an ion exchange group, and for example, the above-mentioned fluorine-containing polymer (I) can be used.
[0101] Catalyst layer 1cm 2 The mass of the catalytic metal per 2 More than 0.2 mg / cm is preferred. 2 More preferably, 4 mg / cm 2 Preferably, 2 mg / cm or less 2 More preferably, 1 mg / cm or less 2 The following is more preferred: The mass ratio of the catalyst to the polymer having an ion-exchange group in the catalyst layer (mass of catalyst / mass of polymer having an ion-exchange group) is preferably 2 to 6.
[0102] The gas diffusion layer functions to rapidly diffuse gas generated from the catalyst layer out of the catalyst layer and also functions as a current collector. Specific examples of gas diffusion layers include carbon paper, carbon cloth, carbon felt, sintered titanium oxide fibers, and sintered titanium oxide particles. The anode side has a high potential, and using carbon materials would result in oxidation, so it is preferable to use sintered titanium oxide fibers or sintered titanium oxide particles. The titanium oxide sintered material may be plated with platinum or other metals as needed. The cathode gas diffusion layer may be treated with PTFE or other materials to provide water repellency. While the membrane electrode assembly in FIG. 1 includes a gas diffusion layer 28, the gas diffusion layer is an optional component and may not be included in the membrane electrode assembly.
[0103] The film thickness of the anode and the cathode is preferably 5 μm or more, and is preferably 100 μm or less, more preferably 50 μm or less, even more preferably 30 μm or less, and particularly preferably 15 μm or less, from the viewpoint of obtaining superior effects of the present invention. The film thickness of the anode and the cathode is measured using an image obtained by measuring a cross section of the membrane electrode assembly cut in the film thickness direction with a laser microscope, and is an arithmetic average value at any 20 points.
[0104] <Method for Manufacturing a Membrane Electrode Assembly> The method for manufacturing a membrane electrode assembly involves forming the cathode catalyst layer on one side of an electrolyte membrane and the anode catalyst layer on the other side of the electrolyte membrane. One example of a method for manufacturing a membrane electrode assembly involves using a laminate having an anode catalyst layer and a releasable substrate (e.g., an ETFE sheet) and another laminate having a cathode catalyst layer and a releasable substrate (e.g., an ETFE sheet), bonding catalyst layers to both sides of the electrolyte membrane, and then peeling off the releasable substrate. The laminate may have a gas diffusion layer between the catalyst layer and the releasable substrate. In this case, the gas diffusion layer can be formed on the catalyst layer opposite the electrolyte membrane. The catalyst layer can be manufactured by applying a catalyst layer-forming coating liquid to a predetermined position (e.g., the surface of the releasable substrate) and drying it as necessary. The catalyst layer-forming coating liquid is a liquid in which a polymer having an ion-exchange group and a catalyst are dispersed in a dispersion medium.
[0105] <Uses> The membrane electrode assembly of the present invention is suitably used in a solid polymer water electrolysis device.
[0106] [Water Electrolysis Apparatus] The water electrolysis apparatus of the present invention comprises the membrane electrode assembly described above, a water supply unit that supplies water to the anode catalyst layer side, and a power supply unit that is electrically connected to the anode catalyst layer side and the cathode catalyst layer side. In the water electrolysis apparatus of the present invention, when a DC voltage is applied by the power supply unit while water is supplied to the anode catalyst layer side by the water supply unit, water is decomposed on the anode catalyst layer side to generate oxygen and protons. On the cathode catalyst layer side, the protons that have migrated to the cathode catalyst layer side through the electrolyte membrane obtain electrons to generate hydrogen. The water electrolysis apparatus of the present invention may have the same configuration as known water electrolysis apparatuses (e.g., an oxygen recovery member that recovers the generated oxygen, a hydrogen recovery member that recovers the generated hydrogen), except for the components described above.
[0107] The present invention will be described in detail below with reference to examples. Examples 1 to 11 are working examples, and Examples 12 to 15 are comparative examples. However, the present invention is not limited to these examples.
[0108] [Ion exchange capacity of fluoropolymer] The fluoropolymer was placed in a glove box filled with dry nitrogen for 24 hours, and the dry mass of the fluoropolymer was measured. Thereafter, the fluoropolymer was immersed in a 2 mol / L aqueous sodium chloride solution at 60°C for 1 hour. The fluoropolymer was washed with ultrapure water and then removed. The solution in which the fluoropolymer had been immersed was titrated with a 0.1 mol / L aqueous sodium hydroxide solution to determine the ion exchange capacity (milli-equivalent / gram dry resin) of the fluoropolymer.
[0109] [Method for measuring the fineness of spun yarn] The weight of the spun yarn is measured using a precision electronic balance, and the fineness (dtex) is calculated using the following formula: Fineness = (10,000 × weight (g)) / length (m)
[0110] [Maximum Frequency Peak in Fiber Diameter Distribution Histogram of Fibers Constituting Nonwoven Fabric (or Woven Fabric)] Nonwoven fabrics A1 to A6, and A9, described below, were observed using a scanning electron microscope at 20,000x magnification, and the fiber diameters of 100 fibers were measured. A fiber diameter distribution histogram was created from the obtained number distribution for each fiber diameter (class width: 20 nm). In the created fiber diameter distribution histogram, the class with the highest frequency was adopted as the maximum frequency peak. The fiber diameter corresponding to the maximum frequency peak was taken as the lower limit fiber diameter of the class with the highest frequency. Furthermore, woven fabrics A7 and nonwoven fabric A8, described below, were observed using a microscope at 300x magnification, and the fiber diameters of 100 fibers were measured. A fiber diameter distribution histogram was created from the obtained number distribution for each fiber diameter (class width: 1,000 nm). In the created fiber diameter distribution histogram, the highest frequency class was adopted as the maximum frequency peak. The fiber diameter corresponding to the maximum frequency peak was taken as the lower limit fiber diameter of the class with the highest frequency.
[0111] [Basis weight of nonwoven fabric (or woven fabric)] A nonwoven fabric (or woven fabric) was cut into a length of 0.15 m and a width of 0.15 m, and the mass was measured using a precision electronic balance. 2 The value converted into the mass per unit area is the basis weight (g / m) of the nonwoven fabric (or woven fabric). 2 )
[0112] [Thickness of Nonwoven Fabric (or Woven Fabric)] The nonwoven fabric was placed on a Dial Gauge Stand 7002 (Mitsutoyo), and the thickness of the nonwoven fabric (or woven fabric) was measured using a Digital Gauge 543-250 (Mitsutoyo) equipped with a flat terminal with a diameter of 5 mm at the tip.
[0113] [Thickness of Electrolyte Membrane] The thickness of each electrolyte membrane was measured using a magnified image (objective lens magnification: 50x) of the cross section of the electrolyte membrane photographed using a laser microscope (product name "VK-X1000", manufactured by Keyence Corporation) under conditions of a temperature of 23°C and a relative humidity of 50% RH.
[0114] [Surface Properties of Electrolyte Membrane] The surface properties of the electrolyte membrane were evaluated by photographing a 3 cm square piece of the electrolyte membrane at a temperature of 25°C and a relative humidity of 50% RH using a laser microscope (product name "VK-X1000", manufactured by Keyence Corporation) and using the following criteria: ◯: No exposed nonwoven fabric is observed on the surface of the electrolyte membrane ×: Exposed nonwoven fabric is observed on the surface of the electrolyte membrane Note that, for Example 12, it was observed whether exposed woven fabric was observed.
[0115] [Strength] The electrolyte membrane was immersed in pure water and left in an oven at 80°C for 16 hours. After leaving it at room temperature for 3 hours or more, the electrolyte membrane was punched out using a No. 7 dumbbell to prepare a test specimen in a hydrated state of the electrolyte membrane. The test specimen was clamped between chucks and subjected to a tensile test using a TENSILON RTI-1225 (A&D Co., Ltd.) at a speed of 50 mm / min in an oven set at 80°C and a relative humidity of 90%. The elastic modulus was calculated from the obtained stress-strain curve and evaluated according to the following criteria. The tensile test was performed by pulling the nonwoven fabric or woven fabric in the MD direction. ◯: Elastic modulus of 15 MPa or more ×: Elastic modulus of less than 15 MPa
[0116] [Film resistance] The membrane electrode assembly was sandwiched between platinum-plated titanium fiber sintered bodies (manufactured by Bekaert) with a thickness of 0.25 mm and a porosity of 60%, and a platinum-plated titanium plate with a straight flow path was used as a separator. The electrode area was 16 cm. 2The membrane electrode assembly was incorporated into a single cell of 1.0 μS / cm and was evaluated. The membrane electrode assembly was clamped so that a pressure of 1.5 MPa was applied to the electrode portions when sandwiching the membrane electrode assembly. Next, in order to sufficiently hydrate the electrolyte membrane and both electrode ionomers, pure water with a conductivity of 1.0 μS / cm or less, a temperature of 60°C, and atmospheric pressure was supplied to the anode catalyst layer side and the cathode catalyst layer side at a flow rate of 50 mL / min for 8 hours. Thereafter, the water supply to the cathode catalyst layer side was stopped, and pure water with a conductivity of 1.0 μS / cm or less and a temperature of 60°C was supplied to the anode catalyst layer side at a flow rate of 50 mL / min. While maintaining the back pressure at atmospheric pressure for both the anode catalyst layer and the cathode catalyst layer, a current of 16 A (current density 1 A / cm) was applied using a large current potentiostat / galvanostat HCP-803 (manufactured by Biologic). 2 ) for 4 hours as a break-in operation, water electrolysis was carried out. 2 Electrochemical impedance measurement was performed under current control while maintaining a current of 70 mOhm cm, and the membrane resistance was determined. In the Nyquist plot obtained by the electrochemical impedance measurement, the membrane resistance was calculated by multiplying the real part of the impedance at the point where the absolute value of the imaginary part of the impedance is smallest on the high frequency side by the electrode area, and the membrane resistance was evaluated according to the following criteria: ○: 70 mOhm cm 2 Greater than ×: 70 mOhm cm 2 below
[0117] <Production of Fluorine-Containing Polymer (I1)> CF 2 =CF 2 and a compound represented by the following formula (X) (hereinafter also referred to simply as "monomer (X)") were copolymerized to obtain a fluorine-containing polymer (I1) (ion exchange capacity: 1.25 meq / g dry resin). 2 =CF-O-CF 2 CF (CF 3 )-O-CF 2 CF 2 -SO 2 F...Formula (X)
[0118] <Production of Fluorine-Containing Polymer (I2)> CF 2 =CF 2and a compound represented by the following formula (Y) (hereinafter also simply referred to as "monomer (Y)") were copolymerized to obtain a fluorine-containing polymer (I2) (ion exchange capacity: 1.80 meq / g dry resin).
[0119] Formula (Y)
[0120]
[0121] <Production of Fluorine-Containing Polymer (I3)> CF 2 =CF 2 and monomer (X) to obtain a fluorine-containing polymer (I3) (ion exchange capacity: 1.00 meq / g dry resin).
[0122] <Production of Fluorine-Containing Polymer (I4)> CF 2 =CF 2 and monomer (X) to obtain a fluorine-containing polymer (I4) (ion exchange capacity: 1.10 meq / g dry resin).
[0123] <Production of film-attached substrate Y1> A fluoropolymer (I1) was adhered to a substrate made of polyethylene terephthalate by a melt extrusion method to obtain a film-attached substrate Y1 in which a film α1 (film thickness: 30 μm) made of the fluoropolymer (I1) was formed on the substrate.
[0124] <Production of film-attached substrate Y2> A fluoropolymer (I1) was adhered to a substrate made of polyethylene terephthalate by a melt extrusion method, thereby obtaining a film-attached substrate Y2 in which a film α2 (film thickness: 15 μm) made of the fluoropolymer (I1) was formed on the substrate.
[0125] <Production of film-attached substrate Y3> A fluoropolymer (I1) was adhered to a substrate made of polyethylene terephthalate by a melt extrusion method, thereby obtaining a film-attached substrate Y3 in which a film α3 (film thickness: 45 μm) made of the fluoropolymer (I1) was formed on the substrate.
[0126] <Production of film-attached substrate Y4> A fluoropolymer (I2) was adhered to a substrate made of polyethylene terephthalate by a melt extrusion method, thereby obtaining a film-attached substrate Y4 in which a film α4 (film thickness: 30 μm) made of the fluoropolymer (I2) was formed on the substrate.
[0127] <Production of film-attached substrate Y5> A fluoropolymer (I3) was adhered to a substrate made of polyethylene terephthalate by a melt extrusion method, thereby obtaining a film-attached substrate Y5 in which a film α5 (film thickness: 30 μm) made of the fluoropolymer (I3) was formed on the substrate.
[0128] <Production of film-attached substrate Y6> A fluoropolymer (I4) was adhered to a substrate made of polyethylene terephthalate by a melt extrusion method, thereby obtaining a film-attached substrate Y6 in which a film α6 (film thickness: 30 μm) made of the fluoropolymer (I4) was formed on the substrate.
[0129] <Production of film-attached substrate Y7> Fluorine-containing polymer (I1) and cerium oxide were kneaded and pelletized in a twin-screw extruder so that the concentration of cerium oxide was 0.7 wt %. Using the pellets, cerium oxide and fluorine-containing polymer (I1) were adhered to a substrate made of polyethylene terephthalate by melt extrusion, thereby obtaining film-attached substrate Y7 in which a film α7 (film thickness: 30 μm) containing fluorine-containing polymer (I1) and cerium oxide was formed on the substrate.
[0130] <Production of film-attached substrate Y8> Fluorine-containing polymer (I1), cerium oxide, and platinum powder were kneaded and pelletized in a twin-screw extruder so that the concentration of cerium oxide was 0.7 wt% and the concentration of platinum was 0.1 wt%. Using the pellets, cerium oxide, platinum, and the fluorine-containing polymer (I1) were adhered to a substrate made of polyethylene terephthalate by melt extrusion, thereby obtaining film-attached substrate Y8 in which a film α8 (film thickness: 30 μm) made of the fluorine-containing polymer (I1), cerium oxide, and platinum was formed on the substrate.
[0131] <Production of Nonwoven Fabric A1> Polyphenylene sulfide synthesized by a known synthesis method is used as the island component, and polyethylene terephthalate obtained by copolymerizing 5-sodium sulfoisophthalic acid and polyethylene glycol is used as the sea component. The polyphenylene sulfide for the island component is melted at 340°C, and the polyethylene terephthalate for the sea component is melted at 280°C. The molten island component and sea component fibers are merged in a spinneret with 720 islands in the spinneret so that the mass ratio of islands to sea is 70:30, and an islands-in-sea composite fiber is extruded at a spinning temperature of 320°C. The fiber is then treated in a heating zone below the spinneret with a heating length of 90 mm and an atmospheric temperature of 450°C, and a cooling device, oiled, and wound up at a spinning speed of 1000 m / min. The resulting undrawn yarn is adjusted in the spinning discharge flow rate and draw ratio so that the fineness becomes 5 dtex, to obtain a drawn yarn. The resulting drawn yarn is cut to a length of 0.3 mm and immersed in a 5% by mass aqueous solution of sodium hydroxide at 80°C for 30 minutes to remove the sea component, thereby obtaining PPS fiber with an average fiber diameter of approximately 700 nm. 80 wt% of PPS fiber and 20 wt% of undrawn PPS fiber with a fiber diameter of 6 μm are blended together and water is added to prepare a slurry, which is wet-laid, dried, and then crushed by hot calendering to obtain a basis weight of 20 g / m. 2 A nonwoven fabric A1 having a thickness of 37 μm is prepared.
[0132] <Production of Nonwoven Fabric A2> PPS fibers were produced in the same manner as for Nonwoven Fabric A1, and the processing speed during wet papermaking was adjusted to produce a nonwoven fabric with a basis weight of 10 g / m 2 A nonwoven fabric A2 having a thickness of 19 μm is obtained.
[0133] <Production of Nonwoven Fabric A3> Spinning was performed in the same manner as for Nonwoven Fabric A1, except that the number of islands during spinning was changed to 980, the mass ratio of islands to sea was changed to 10:90, and the fineness of the drawn yarn was changed to 1 dtex, to obtain PPS fibers with an average fiber diameter of 100 nm. 80 wt% of the obtained PPS fibers and 20 wt% of undrawn PPS fibers with a fiber diameter of 6 μm were blended, and water was added to prepare a slurry, which was then processed by a wet papermaking method to obtain a basis weight of 20 g / m. 2 A nonwoven fabric A3 having a thickness of 37 μm is prepared.
[0134] <Production of Nonwoven Fabric A4> PPS fibers with an average fiber diameter of 900 nm were obtained by spinning in the same manner as Nonwoven Fabric A1, except that the number of islands during spinning was changed to 400. 80 wt % of the obtained PPS fibers and 20 wt % of unstretched PPS fibers with a fiber diameter of 6 μm were blended, and water was added to prepare a slurry. The slurry was then spun by a wet papermaking method to a basis weight of 20 g / m. 2 A nonwoven fabric A4 having a thickness of 37 μm is prepared.
[0135] <Production of Nonwoven Fabric A5> Spinning was performed in the same manner as for Nonwoven Fabric A1, except that the number of islands during spinning was changed to 950, the mass ratio of islands to sea was changed to 40:60, and the fineness of the drawn yarn was changed to 3.8 dtex, to obtain PPS fibers with an average fiber diameter of 395 nm. 80 wt% of the obtained PPS fibers and 20 wt% of undrawn PPS fibers with a fiber diameter of 6 μm were blended, and water was added to prepare a slurry, which was then subjected to a wet papermaking process to obtain a basis weight of 20 g / m. 2 A nonwoven fabric A5 having a thickness of 37 μm is prepared.
[0136] <Production of Nonwoven Fabric A6> PPS fibers were produced in the same manner as for Nonwoven Fabric A1. The obtained PPS fibers were mixed with water to prepare a slurry, and the pressure of thermal calendering was adjusted by a wet papermaking method to produce a nonwoven fabric having a basis weight of 20 g / m 2 A nonwoven fabric A6 having a thickness of 61 μm is obtained.
[0137] <Production of Woven Fabric A7> Woven fabric A7 was obtained by plain weaving 18.6 denier PFA yarns as warp and weft yarns so that the density of the PFA yarns was 100 threads / inch. The weight of the woven fabric A7 was 16.3 g / m 2 It was.
[0138] <Production of Nonwoven Fabric A8> Polyphenylene sulfide was melted at 340°C and spun using a spinning device to obtain an undrawn yarn with a fineness of 2.0 detx. The obtained undrawn yarn was drawn to obtain a drawn PPS yarn with an average fiber diameter of 10,000 nm. The obtained drawn PPS fiber and the undrawn PPS fiber were blended at 60 wt% and 40 wt%, respectively, and water was added to prepare a slurry. The slurry was then spun by a wet papermaking method to obtain a basis weight of 10 g / m. 2 A nonwoven fabric A8 having a thickness of 18 μm was produced.
[0139] <Production of Nonwoven Fabric A9> Polyethersulfone (PES) polymerized by a known method was dissolved in dimethylacetamide to a solids concentration of 25 wt %. The resulting solution was fed into an electrospinning device with an inner diameter of 0.44 mm and a distance from the metal plate of 5.5 cm, and spun at a resin discharge rate of 17 mg / min and an applied voltage of 12 kV to produce fibers. The fibers were collected on the surface of the metal plate, resulting in a fiber with an average fiber diameter of 350 nm and a basis weight of 3.2 g / m. 2 A nonwoven fabric A9 having a thickness of 15 μm was produced.
[0140] <Preparation of Cathode Catalyst Layer Decal> Water (59.4 g) and ethanol (39.6 g) were added to 11 g of a supported catalyst (manufactured by Tanaka Kikinzoku Kogyo Co., Ltd.) containing 46% platinum by mass supported on carbon powder ("TEC10E50E"), and the mixture was mixed and pulverized using an ultrasonic homogenizer to obtain a catalyst dispersion. To the catalyst dispersion, a dispersion (20.1 g) of a polymer (ion exchange capacity: 1.10 meq / g dry resin) copolymerized with TFE and monomer (X) and converted to an acid form through hydrolysis and acid treatment in a water / ethanol = 40 / 60 (mass%) solvent at a solids concentration of 26.0% (hereinafter also referred to as "Dispersion Y"), ethanol (11 g), and Zeorora-H (manufactured by Nippon Zeon Co., Ltd.) (6.3 g) were added. Further, water (3.66 g) and ethanol (7.63 g) were added to the obtained dispersion and mixed for 60 minutes using a paint conditioner to adjust the solid content concentration to 10.0 mass % to obtain a cathode catalyst ink. The cathode catalyst ink was applied to an ETFE sheet using a die coater, dried at 80°C, and further subjected to heat treatment at 150°C for 15 minutes to obtain a cathode catalyst ink having a platinum content of 0.4 mg / cm. 2 As a result, a cathode catalyst layer decal of 1000 nm was obtained.
[0141] <Preparation of anode catalyst layer decal> Ethanol (18.06 g) and Zeororah-H (manufactured by Zeon Corporation) (10.58 g) were added to dispersion Y (33.0 g), and the mixture was mixed for 5 minutes at 2200 rpm using a planetary centrifugal mixer (Thinky's Awatori Rentaro). Ethanol (46.44 g) and water (75.75 g) were added to the mixed composition (54.06 g), and the mixture was mixed with a 100 m2 anode catalyst layer decal containing 74.8% by mass of iridium. 240.0 g of an iridium oxide catalyst (manufactured by Tanaka Kikinzoku Kogyo Co., Ltd.) was added to the mixture. The resulting mixture was processed in a planetary bead mill (rotational speed: 300 rpm) for 90 minutes to obtain an anode catalyst ink with a solids concentration of 22 mass %. The anode catalyst ink was applied to an ETFE sheet so that the iridium concentration was 1.0 mg / cm. 2 The anode catalyst layer decal was obtained by applying the coating with an applicator so that the coating became smooth, followed by drying at 80° C. for 10 minutes and then heat treating at 150° C. for 15 minutes.
[0142] [Example 1] Film-attached substrate Y1 / nonwoven fabric A1 / film-attached substrate Y1 are stacked in this order. The film-attached substrate Y1 is positioned so that the film α1 in the film-attached substrate Y1 is in contact with the nonwoven fabric A1. The stacked components are heated and pressed for 5 minutes using a flat press under conditions of a temperature of 200 ° C and a surface pressure of 5 MPa, and the substrates on both sides are peeled off at a temperature of 50 ° C to obtain a precursor membrane. The precursor membrane is immersed in a solution of dimethyl sulfoxide / potassium hydroxide / water = 30 / 5.5 / 64.5 (mass ratio) at 80 ° C for 16 hours, and the groups in the precursor membrane that can be converted to sulfonic acid functional groups are hydrolyzed to K-type sulfonic acid functional groups, and then washed with water. The membrane is then immersed in a 3M aqueous hydrochloric acid solution to convert the terminal groups from K-type to H-type, washed with water, and dried to obtain an electrolyte membrane X1 (thickness 60 μm). The resulting electrolyte membrane is subjected to evaluation of surface properties and mechanical strength. The results are shown in Table 1. The catalyst layer of the anode catalyst layer decal cut to 4 cm x 4 cm was placed face-to-face with one surface of the electrolyte membrane X1 cut to 7 cm x 7 cm, and the catalyst layer of the cathode catalyst layer decal cut to 4 cm x 4 cm was placed face-to-face with the other surface of the electrolyte membrane X1, and the membrane was hot-pressed at a press temperature of 150°C for 10 minutes under a pressure of 3 MPa. After the temperature was lowered to 70°C, the pressure was released and the membrane was removed. The ETFE sheets of the anode catalyst layer decal and the cathode catalyst layer decal were peeled off, and the membrane was heated to an electrode area of 16 cm. 2 The membrane electrode assembly thus obtained was subjected to evaluation of membrane resistance. The evaluation results are shown in Tables 1 and 2.
[0143] Examples 2 to 15 Electrolyte membranes and membrane electrode assemblies were obtained in the same manner as in Example 1, except that the film-attached substrate and nonwoven fabric or woven fabric used were changed to the types shown in Table 1 below. Various evaluations were performed using the obtained electrolyte membranes and membrane electrode assemblies. The evaluation results are shown in Tables 1 and 2.
[0144] In Tables 1 and 2, "X" in the "Structural Unit" column represents the monomer (X), and "Y" represents the monomer (Y). In Tables 1 and 2, "Ce" in the "Additive" column represents cerium, and "Pt" represents platinum.
[0145]
[0146]
[0147] As shown in the above table, it was confirmed that the solid polymer electrolyte membrane of the present invention exhibits the desired effects. The entire contents of the specification, claims, drawings, and abstract of Japanese Patent Application No. 2023-052010, filed on March 28, 2023, are incorporated herein by reference as part of the disclosure of the present invention.
[0148] 10 Electrolyte membrane 20 Membrane electrode assembly 22 Anode 24 Cathode 26 Catalyst layer 28 Gas diffusion layer
Claims
1. A solid polymer electrolyte membrane comprising a fluorine-containing polymer having ion exchange groups and a nonwoven fabric, wherein the nonwoven fabric contains polyphenylene sulfide fibers, a fiber diameter distribution histogram of the fibers constituting the nonwoven fabric has a maximum frequency peak in the range of 100 to 900 nm, and the thickness of the solid polymer electrolyte membrane is 30 to 90 μm.
2. The solid polymer electrolyte membrane according to claim 1, wherein the ion exchange group of the fluorine-containing polymer is a sulfonic acid type functional group.
3. The solid polymer electrolyte membrane according to claim 1, wherein the fluoropolymer contains at least one unit selected from the group consisting of a unit represented by formula (1-1), a unit represented by formula (1-2), a unit represented by formula (1-3), and a unit represented by formula (1-4). 2 -CF(-O-R f1 -SO 3 M)] - Formula (1-2) - [CF 2 -CF(-R f1 -SO 3 M) ]- R f1 is a perfluoroalkylene group which may contain an oxygen atom between the carbon atoms, and R f2 is a single bond or a perfluoroalkylene group which may contain an oxygen atom between carbon atoms, and R f3 represents a single bond or a perfluoroalkylene group which may contain an oxygen atom between carbon atoms, r is 0 or 1, m is 0 or 1, and M is a hydrogen atom, an alkali metal, or a quaternary ammonium cation.
4. The solid polymer electrolyte membrane according to claim 1, which contains at least one element selected from the group consisting of platinum, palladium, cerium, and manganese.
5. The solid polymer electrolyte membrane according to claim 1, wherein the content of the nonwoven fabric is 5 mass % or more and 40 mass % or less based on the total mass of the solid polymer electrolyte membrane.
6. The solid polymer electrolyte membrane according to claim 1, which is used for water electrolysis.
7. A membrane electrode assembly comprising: the solid polymer electrolyte membrane according to any one of claims 1 to 6; a cathode catalyst layer disposed on one side of the solid polymer electrolyte membrane; and an anode catalyst layer disposed on the other side of the solid polymer electrolyte membrane.
8. A water electrolysis device comprising: the membrane electrode assembly according to claim 7; a power supply unit connected to the cathode catalyst layer side and the anode catalyst layer side of the membrane electrode assembly; and a water supply unit that supplies water to the anode catalyst layer side.
9. A method for producing a solid polymer electrolyte membrane according to any one of claims 1 to 6, comprising: step 1 of converting groups convertible to ion-exchange groups in a precursor membrane comprising a polymer having groups convertible to ion-exchange groups and the nonwoven fabric into ion-exchange groups; and step 2 of drying the membrane obtained in step 1 while restraining the periphery thereof to obtain the solid polymer electrolyte membrane.
10. The method for producing a solid polymer electrolyte membrane according to claim 9, further comprising, before step 1, step 3 of sandwiching a nonwoven fabric between a plurality of polymer membranes containing a polymer having a group that can be converted into an ion-exchange group to obtain the precursor membrane.
11. The method for producing a solid polymer electrolyte membrane according to claim 10, further comprising, before step 3, step 4 of kneading a compound containing at least one element selected from the group consisting of platinum, palladium, cerium, and manganese with a polymer having a group that can be converted into an ion-exchange group, and extruding the resulting kneaded mixture to obtain the precursor membrane.
Citation Information
Patent Citations
Polymer electrolyte composition containing aromatic hydrocarbon resins
JP4447007B2
Composite polymer electrolyte membrane and method for producing the same
JP5867093B2
Diaphragm for electrolyzing alkaline water, and device for electrolyzing alkaline water
WO2018070444A1
Solid polymer electrolyte film, membrane electrode assembly and electrolyzer
WO2019088299A1