Inkjet composition for forming partition wall, LED module and method for manufacturing LED module

The inkjet composition for forming partition walls around LED chips addresses the issues of reflow resistance and thermal stability by using a specific formulation of photocurable and thermosetting compounds, improving mechanical strength and adhesion, and maintaining contact with reflective films.

WO2024204093A1PCT designated stage expired Publication Date: 2024-10-03SEKISUI CHEMICAL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011754
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-25
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional inkjet compositions fail to effectively form partition walls around LED chips due to low reflow resistance and poor thermal cycle characteristics, leading to peeling or cracking issues when subjected to repeated cooling and heating.

Method used

An inkjet composition comprising a photocurable compound with photocurable and thermosetting functional groups, a thermosetting compound, a photopolymerization initiator, a thermosetting agent, and an antioxidant, which is applied using an inkjet device to form partition walls that improve reflow resistance and thermal cycle characteristics.

Benefits of technology

The inkjet composition enhances the mechanical strength and adhesion of partition walls, preventing peeling and cracking during reflow and maintaining high mechanical strength and adhesion even after repeated cooling and heating cycles, while also ensuring good contact with reflective films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011754_03102024_PF_FP_ABST
    Figure JP2024011754_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides an inkjet composition for forming a partition wall, the inkjet composition having enhanced reflow resistance and enhanced temperature cycle characteristics. An inkjet composition for forming a partition wall according to the present invention contains: a photocurable compound which has a photocurable functional group, while having or not having a thermosetting functional group; a thermosetting compound which has a thermosetting functional group, while having no photocurable functional group; a photopolymerization initiator; a thermal curing agent; and an antioxidant. The thermosetting compound is in a liquid state at 25°C.
Need to check novelty before this filing date? Find Prior Art

Description

Inkjet composition for partition wall formation, LED module, and method for manufacturing LED module

[0001] The present invention relates to an inkjet composition for partition wall formation that is applied using an inkjet device.The present invention also relates to an LED module using the inkjet composition for partition wall formation.The present invention also relates to a method for manufacturing an LED module using the inkjet composition for partition wall formation.

[0002] Light-emitting diode (LED) devices including LED chips are widely used. In order to improve the extraction efficiency of light emitted from the LED chip, methods of providing a partition wall or a reflective layer around the periphery of the LED chip have been investigated.

[0003] For example, Patent Document 1 below discloses a method for manufacturing an LED device having a substrate, an LED element mounted on the substrate, a wavelength conversion layer covering the LED element, and a reflective layer formed on the substrate and outside the periphery of the mounting area of ​​the LED element. This manufacturing method includes the following steps: (1) a mounting step of mounting the LED element on the substrate; (2) a reflective layer forming step of applying a reflective layer forming composition containing light-diffusing particles, an organosilicon compound, and a solvent onto the substrate, and drying and curing the reflective layer forming composition to form the reflective layer; and (3) a wavelength conversion layer forming step of applying a wavelength conversion layer forming composition containing phosphor particles and a binder component so as to cover the LED element, thereby forming the wavelength conversion layer.

[0004] Japanese Patent Application Laid-Open No. 2014-158011

[0005] A conventional method for forming partition walls involves using a dry film resist, developing it, and then plating it, but this method requires multiple exposure and development steps, resulting in poor productivity.

[0006] Another possible method for forming a partition wall on the periphery of an LED chip is to use an inkjet device to apply an inkjet composition in a frame shape and then cure the applied inkjet composition to form the partition wall.

[0007] However, since conventional inkjet compositions are not intended to be used for forming partition walls, they may not be able to form partition walls well. Furthermore, even if conventional inkjet compositions can form partition walls well to some extent, they may have low reflow resistance. Therefore, after reflow, the partition walls may peel off from the substrate or cracks may occur in the partition walls.

[0008] Furthermore, when partition walls formed using a conventional inkjet composition are repeatedly cooled and heated, the partition walls may peel off from the substrate or cracks may occur due to repeated expansion and contraction, which means that it is difficult to improve the cooling-heating cycle properties of the conventional inkjet composition.

[0009] An object of the present invention is to provide an inkjet composition for forming a partition wall that can improve reflow resistance and thermal cycle characteristics. Another object of the present invention is to provide an LED module using the inkjet composition for forming a partition wall. Another object of the present invention is to provide a method for manufacturing an LED module using the inkjet composition for forming a partition wall.

[0010] This specification discloses the following ink jet composition for forming a partition wall, an LED module, and a method for manufacturing an LED module.

[0011] Item 1. An inkjet composition for forming a partition wall, comprising: a photocurable compound having a photocurable functional group and either having or not having a thermocurable functional group; a thermosetting compound having no photocurable functional group and a thermosetting functional group; a photopolymerization initiator; a heat curing agent; and an antioxidant, wherein the thermosetting compound is liquid at 25°C.

[0012] Item 2. The ink jet composition for forming partition walls according to Item 1, wherein the antioxidant includes a phenol-based antioxidant.

[0013] Item 3. The ink jet composition for forming partition walls according to Item 1 or 2, wherein the thermosetting compound contains a bisphenol A epoxy compound or a bisphenol F epoxy compound.

[0014] Item 4. The ink jet composition for forming partition walls according to any one of Items 1 to 3, wherein the photocurable compound includes a photocurable compound having two or more (meth)acryloyl groups and an alicyclic skeleton.

[0015] Item 5. The ink jet composition for forming partition walls according to any one of Items 1 to 4, wherein the photocurable compound includes a photocurable compound having two or more (meth)acryloyl groups and a dicyclopentadiene skeleton.

[0016] Item 6. The ink jet composition for forming a partition wall according to any one of Items 1 to 5, wherein the content of the photocurable compound is 40% by weight or more and 75% by weight or less, based on 100% by weight of the ink jet composition for forming a partition wall.

[0017] Item 7. The ink jet composition for forming a partition wall according to any one of Items 1 to 6, wherein the content of the thermosetting compound is 10% by weight or more and 35% by weight or less, based on 100% by weight of the ink jet composition for forming a partition wall.

[0018] Item 8. The ink jet composition for forming a partition wall according to any one of Items 1 to 7, wherein the content of the antioxidant is 0.3 wt % or more and 4 wt % or less, based on 100 wt % of the ink jet composition for forming a partition wall.

[0019] Item 9. The ink jet composition for forming a partition wall according to any one of Items 1 to 8, wherein the photopolymerization initiator includes an aminoacetophenone-based photopolymerization initiator.

[0020] Item 10. The ink jet composition for forming partition walls according to any one of Items 1 to 9, wherein the heat curing agent contains an aromatic amine compound.

[0021] Item 11. The ink jet composition for forming partition walls according to any one of Items 1 to 10, wherein the heat curing agent contains 1,3-bis(3-aminophenoxy)benzene or bis[4-(3-aminophenoxy)phenyl]sulfone.

[0022] Item 12. An LED module comprising: a substrate; an LED chip disposed on a first surface of the substrate; and a partition wall disposed on the first surface of the substrate, wherein the partition wall is disposed on the first surface of the substrate so as to surround the LED chip, and the partition wall is a cured product of the inkjet composition for forming a partition wall according to any one of Items 1 to 11.

[0023] Item 13. The LED module according to Item 12, further comprising a reflective film on the inner wall surface of the partition wall.

[0024] Item 14. A method for manufacturing an LED module, comprising the steps of: using an electronic component including a substrate and an LED chip arranged on a first surface of the substrate, applying the inkjet composition for partition wall formation according to any one of Items 1 to 11 onto the first surface of the substrate in the electronic component by inkjet printing to form an inkjet composition layer; and curing the inkjet composition layer to form a partition wall on the first surface of the substrate, wherein in the obtained LED module, the partition wall is arranged on the first surface of the substrate so as to surround the LED chip, and the partition wall is a cured product of the inkjet composition for partition wall formation.

[0025] Item 15. The method for manufacturing an LED module according to Item 14, further comprising the step of disposing a reflective film on an inner wall surface of the partition wall.

[0026] The ink jet composition for partition wall formation according to the present invention comprises a photocurable compound having a photocurable functional group and either a thermosetting functional group or not, a thermosetting compound having either a photocurable functional group or not, a photopolymerization initiator, a heat curing agent, and an antioxidant. In the ink jet composition for partition wall formation according to the present invention, the thermosetting compound is liquid at 25°C. Because the ink jet composition for partition wall formation according to the present invention has the above-mentioned configuration, it is possible to improve reflow resistance and thermal cycle properties.

[0027] Fig. 1(a) is a plan view schematically showing an LED module obtained using an ink jet composition for partition wall formation according to a first embodiment of the present invention, and Fig. 1(b) is a cross-sectional view schematically showing the LED module. Fig. 2 is a cross-sectional view schematically showing an LED module obtained using an ink jet composition for partition wall formation according to a second embodiment of the present invention.

[0028] The present invention will be described in detail below.

[0029] (Inkjet Composition for Partition Wall Formation) The inkjet composition for partition wall formation according to the present invention (hereinafter, may be referred to as "inkjet composition") is used for inkjet coating.

[0030] The ink jet composition according to the present invention comprises the following components:

[0031] (A) a photocurable compound having a photocurable functional group and having or not having a thermosetting functional group (hereinafter, this may be referred to as "(A) photocurable compound"); (B) a thermosetting compound having no photocurable functional group and having a thermosetting functional group (hereinafter, this may be referred to as "(B) thermosetting compound"); (C) a photopolymerization initiator; (D) a thermosetting agent; and (E) an antioxidant.

[0032] In the ink jet composition according to the present invention, the thermosetting compound (B) is liquid at 25°C.

[0033] The inkjet composition has photocurability and thermosetting properties. The inkjet composition is a curable composition for inkjet printing and for forming partition walls. The inkjet composition is preferably cured by irradiation with light and heating before use. More preferably, the inkjet composition is cured by heating after curing has been promoted by irradiation with light.

[0034] The inkjet composition can be applied by an inkjet method. When applying the inkjet composition by the inkjet method, an inkjet device is used. The inkjet device has an inkjet head. The inkjet head has an inkjet nozzle. The inkjet composition is different from compositions applied by screen printing and compositions applied by a dispenser.

[0035] The inkjet composition according to the present invention has the above-described configuration, and therefore can improve reflow resistance. The inkjet composition according to the present invention can increase the mechanical strength of the partition walls obtained and improve the adhesion between the substrate and the partition walls. More specifically, the inkjet composition according to the present invention can prevent cracks from occurring in the partition walls formed from the inkjet composition and prevent the partition walls from peeling off from the substrate, even when heated by reflow.

[0036] Furthermore, since the inkjet composition according to the present invention has the above-described configuration, it is possible to improve the cooling-heating cycle characteristics. With the inkjet composition according to the present invention, even when cooling and heating are repeatedly performed, the mechanical strength of the partition walls obtained can be maintained high, and the adhesion between the substrate and the partition walls can be maintained high. More specifically, even when cooling and heating are repeatedly performed on the partition walls formed using the inkjet composition, it is possible to prevent the partition walls from peeling off from the substrate and the partition walls from cracking.

[0037]

[0033] Furthermore, since the inkjet composition according to the present invention has the above-mentioned configuration, when a reflective film is formed on the inner wall surface of the partition wall formed using the inkjet composition, the adhesion between the partition wall and the reflective film can be improved. More specifically, when a reflective film is formed on the inner wall surface of the partition wall formed using the inkjet composition, the inkjet composition according to the present invention can prevent the reflective film from peeling off from the partition wall even when heated by reflow.

[0038] The inkjet composition is preferably used, for example, to form partition walls in an LED module. The inkjet composition is preferably used to form partition walls in the gaps between multiple LED chips. The inkjet composition is preferably used to form partition walls around the periphery of the mounting area of ​​an LED chip. This can improve the utilization efficiency of light generated from the LED chip. Note that when the LED chip is an LED chip that emits ultraviolet light (UV-LED chip), the luminous efficiency of the LED chip itself may be low. Since the use of the inkjet composition can improve the light extraction efficiency, the inkjet composition can be particularly preferably used when the LED chip is an LED chip that emits ultraviolet light (UV-LED chip).

[0039] The inkjet composition is particularly suitable for use in COB or COG LED modules, and more preferably used as an inkjet composition for forming partition walls in COB or COG LED modules.

[0040] From the viewpoint of more effectively applying the inkjet composition by the inkjet method, the inkjet composition is preferably in a liquid state at 25° C. The liquid state also includes a paste state.

[0041] The viscosity (η25) of the inkjet composition at 25° C. is preferably 20 mPa·s or more, more preferably 100 mPa·s or more, even more preferably 150 mPa·s or more, and is preferably 1500 mPa·s or less, more preferably 1000 mPa·s or less, even more preferably 800 mPa·s or less. When the viscosity (η25) is equal to or more than the above lower limit and equal to or less than the above upper limit, the inkjet ejection properties can be further improved.

[0042] The viscosity (η25) is preferably measured using an E-type viscometer (for example, "TVE22L" manufactured by Toki Sangyo Co., Ltd.) for the ink jet composition immediately after preparation under conditions of 25° C. and 10 rpm.

[0043] When ejected by the inkjet device, the inkjet composition is preferably ejected in a heated state at 40° C. or higher and 100° C. or lower. From the viewpoints of increasing the height precision of the obtained partition walls and making it difficult for voids to occur in the partition walls, it is preferable to apply the inkjet composition while circulating it.

[0044] It is preferable that the inkjet device has an ink tank in which the inkjet composition is stored, a discharge part connected to the ink tank and from which the inkjet composition is discharged, and a circulation flow path part having one end connected to the discharge part and the other end connected to the ink tank and through which the inkjet composition flows.

[0045]

[0023] In the inkjet device, it is preferable to apply the inkjet composition while circulating it by moving the inkjet composition from the ink tank to the ejection section, and then flowing the inkjet composition that has not been ejected from the ejection section into the circulation channel section and moving it to the ink tank. Applying the inkjet composition while circulating it can improve the height precision of the partition walls obtained and make it less likely that voids will occur in the partition walls.

[0046] The glass transition temperature (Tg) of the cured product of the inkjet composition is preferably 80°C or higher, more preferably 95°C or higher, and even more preferably 110°C or higher. When the glass transition temperature (Tg) of the cured product of the inkjet composition is equal to or higher than the above-mentioned lower limit, the thermal cycle properties can be further improved. The upper limit of the glass transition temperature (Tg) of the cured product of the inkjet composition is not particularly limited. The glass transition temperature (Tg) of the cured product of the inkjet composition may be 300°C or lower, or may be 250°C or lower. The range of the glass transition temperature (Tg) of the cured product of the inkjet composition can be set by appropriately selecting the above-mentioned lower limit and upper limit.

[0047] The glass transition temperature of the cured product of the inkjet composition can be measured using a dynamic viscoelasticity measuring device at a temperature rise rate of 10°C / min and a frequency of 10 Hz. Examples of the dynamic viscoelasticity measuring device include "DVA-200" manufactured by IT Measurement & Control Co., Ltd.

[0048] The cured product of the inkjet composition can be obtained, for example, by the following method: After applying the inkjet composition to the surface of a glass substrate using an inkjet device, the inkjet composition is applied to a glass substrate at an illuminance of 1000 mW / cm at a wavelength of 365 nm. 2 The cumulative light intensity was 1000 mJ / cm 2 The ink-jet composition is then irradiated with ultraviolet light (UV-LED) of 1000 W. Thereafter, the ink-jet composition is heated at 170° C. for 3 hours to be thermally cured, thereby forming a cured product of the ink-jet composition.

[0049] Hereinafter, each component contained in the inkjet composition will be described in detail. In this specification, "(meth)acryloyl" means one or both of "acryloyl" and "methacryloyl", and "(meth)acrylate" means one or both of "acrylate" and "methacrylate". In addition, in this specification, the CH 2 =C(H or CH 3 ) groups are not included in the vinyl groups.

[0050] <(A) Photocurable Compound> The (A) photocurable compound is a compound having a photocurable functional group and having or not having a thermosetting functional group. The (A) photocurable compound may or may not have a thermosetting functional group. The (A) photocurable compound may be both a photocurable and thermosetting compound.

[0051] Examples of the photocurable functional group include a (meth)acryloyl group and a vinyl group.

[0052] Examples of the (A) photocurable compound include a compound having a (meth)acryloyl group and a compound having a vinyl group. The (A) photocurable compound may be used alone or in combination of two or more.

[0053] From the viewpoint of enhancing photocurability, the photocurable compound (A) preferably has a (meth)acryloyl group, and the photocurable functional group of the photocurable compound (A) is preferably a (meth)acryloyl group.

[0054] The (A) photocurable compound may be a monofunctional (meth)acrylate or a polyfunctional (meth)acrylate. The (A) photocurable compound may be a bifunctional (meth)acrylate compound, a bifunctional or higher functional (meth)acrylate compound, a trifunctional (meth)acrylate compound, or a trifunctional or higher functional (meth)acrylate compound. The (A) photocurable compound may be a 20- or lower functional (meth)acrylate compound, a 10- or lower functional (meth)acrylate compound, or a 5- or lower functional (meth)acrylate compound.

[0055] The (A) photocurable compound may have one (meth)acryloyl group, two (meth)acryloyl groups, two or more (meth)acryloyl groups, three (meth)acryloyl groups, three or more (meth)acryloyl groups, four (meth)acryloyl groups, four or more (meth)acryloyl groups, 20 or less (meth)acryloyl groups, 10 or less (meth)acryloyl groups, or five or less (meth)acryloyl groups.

[0056] In order to more effectively exert the effects of the present invention, the (A) photocurable compound preferably includes a photocurable compound having two or more (meth)acryloyl groups.

[0057] Examples of the monofunctional (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, sec-butyl (meth)acrylate, t-butyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, allyl (meth)acrylate, benzyl (meth)acrylate, cyclohexyl (meth)acrylate, phenyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, and 2-phenoxyethyl (meth)acrylate, methoxydiethylene glycol (meth)acrylate, methoxytriethylene glycol (meth)acrylate, methoxypropylene glycol (meth)acrylate, methoxydipropylene glycol (meth)acrylate, isobornyl (meth)acrylate, dicyclopentadienyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, glycerol mono(meth)acrylate, 2-ethylhexyl (meth)acrylate, dihydroxycyclopentadienyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, naphthyl (meth)acrylate, lauryl (meth)acrylate, and stearyl (meth)acrylate.

[0058] Examples of the bifunctional (meth)acrylate include 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanedi(meth)acrylate, 1,10-decanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 2,4-dimethyl-1,5-pentanediol di(meth)acrylate, butylethylpropanediol di(meth)acrylate, ethoxylated cyclohexanemethanol di(meth)acrylate, polyethylene glycol di(meth)acrylate, oligoethylene glycol di(meth)acrylate, ethylene glycol di(meth)acrylate, 2-ethyl-2-butylbutanediol di(meth)acrylate, 2-ethyl-2-butylpropanediol di(meth)acrylate, tricyclodecane di(meth)acrylate, and dipropylene glycol di(meth)acrylate.

[0059] Examples of the trifunctional (meth)acrylate include trimethylolpropane tri(meth)acrylate, trimethylolethane tri(meth)acrylate, alkylene oxide-modified tri(meth)acrylate of trimethylolpropane, pentaerythritol tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, trimethylolpropane tri((meth)acryloyloxypropyl)ether, alkylene oxide-modified tri(meth)acrylate of isocyanuric acid, dipentaerythritol propionate tri(meth)acrylate, tri((meth)acryloyloxyethyl)isocyanurate, and sorbitol tri(meth)acrylate.

[0060] Examples of the tetrafunctional (meth)acrylate include pentaerythritol tetra(meth)acrylate, sorbitol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, and dipentaerythritol propionate tetra(meth)acrylate.

[0061] Examples of the pentafunctional (meth)acrylate include sorbitol penta(meth)acrylate and dipentaerythritol penta(meth)acrylate.

[0062] Examples of the hexafunctional (meth)acrylate include dipentaerythritol hexa(meth)acrylate, sorbitol hexa(meth)acrylate, and alkylene oxide-modified hexa(meth)acrylate of phosphazene.

[0063] In order to more effectively exert the effects of the present invention, it is preferable that the (A) photocurable compound contains a photocurable compound having an alicyclic skeleton.

[0064] Examples of the alicyclic skeleton include a dicyclopentadiene skeleton, a cyclopropane skeleton, a cyclobutane skeleton, a cyclopentane skeleton, a cyclohexane skeleton, a cycloheptane skeleton, a cyclooctane skeleton, a cyclononane skeleton, a cyclodecane skeleton, a cycloundecane skeleton, a cyclododecane skeleton, a tetracyclododecene skeleton, a cubane skeleton, a basketane skeleton, a norbornene skeleton, an adamantane skeleton, and an isobornyl skeleton.

[0065] From the viewpoint of more effectively exerting the effects of the present invention, the alicyclic skeleton is preferably a dicyclopentadiene skeleton. From the viewpoint of more effectively exerting the effects of the present invention, the (A) photocurable compound preferably includes a photocurable compound having two or more (meth)acryloyl groups and an alicyclic skeleton, and more preferably includes a photocurable compound having two or more (meth)acryloyl groups and a dicyclopentadiene skeleton.

[0066] Examples of the photocurable compound having two or more (meth)acryloyl groups and an alicyclic skeleton include ethoxylated cyclohexanemethanol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, 1,3-adamantanediol di(meth)acrylate, propoxylated cyclohexanemethanol di(meth)acrylate, and pentaerythritol triacrylate-isophorone diisocyanate-urethane prepolymer.

[0067] From the viewpoint of more effectively exerting the effects of the present invention, the (A) photocurable compound preferably contains 1,3-adamantanediol di(meth)acrylate or tricyclodecane dimethanol di(meth)acrylate, and more preferably contains tricyclodecane dimethanol di(meth)acrylate.

[0068] From the viewpoint of more effectively exerting the effects of the present invention, particularly from the viewpoint of further improving thermal cycling properties, it is preferable that the photocurable compound (A) contains a cyclopolymerizable compound.

[0069] The cyclopolymerizable compound is a compound capable of cyclopolymerization. The cyclopolymerizable compound has a cyclopolymerizable group. The cyclopolymerizable compound is capable of forming a polymer having a cyclic skeleton. It is preferable that the cyclopolymerizable compound is capable of forming a polymer having a cyclic skeleton in the main chain.

[0070] The cyclopolymerizable compound is preferably cyclized by radical polymerization. The cyclopolymerizable compound is preferably capable of forming a polymer having a cyclic skeleton by radical polymerization, more preferably capable of forming a polymer having a cyclic skeleton in the main chain by radical polymerization. In the cyclopolymerizable compound, it is preferable that the radical polymerization reaction proceeds while cyclizing.

[0071]

[0033] From the viewpoint of increasing the adhesive strength between the substrate and the cured product of the inkjet composition and further improving the thermal cycling properties, the cyclopolymerizable compound is preferably capable of forming a 5-membered ring structure or a 6-membered ring structure, and more preferably capable of forming a 5-membered ring ether structure or a 6-membered ring ether structure. From the viewpoint of increasing the adhesive strength between the substrate and the cured product of the inkjet composition and further improving the thermal cycling properties, the cyclopolymerizable compound is preferably capable of forming a 5-membered ring structure, and more preferably capable of forming a 5-membered ring ether structure.

[0072] The cyclopolymerizable compound has a photocurable functional group. The cyclopolymerizable compound is a compound having a photocurable functional group and a cyclopolymerizable group. The cyclopolymerizable compound is a cyclopolymerizable photocurable compound. In the cyclopolymerizable compound, the photocurable functional group may be a part of the cyclopolymerizable group or may be a side chain of the cyclopolymerizable group. In the cyclopolymerizable compound, the photocurable functional group and the cyclopolymerizable group may share some atoms or some skeletons.

[0073] The cyclopolymerizable compound may have 1, 2, 2 or more, 3 or more, 4 or more, 5 or more, or 6 or more cyclopolymerizable groups. The cyclopolymerizable compound may have 12 or less, 8 or less, or 6 or less cyclopolymerizable groups.

[0074]

[0033] From the viewpoint of further enhancing the effects of the present invention, it is preferable that the cyclopolymerizable compound includes a photocurable compound having one cyclopolymerizable group. From the viewpoints of further enhancing the photocurability of the inkjet composition, favorably forming partition walls having a larger aspect ratio, increasing the glass transition temperature (Tg) of the cured product of the inkjet composition, and further enhancing the thermal cycle properties of the cured product of the inkjet composition, it is preferable that the cyclopolymerizable compound includes a photocurable compound having two or more cyclopolymerizable groups.

[0075] The cyclopolymerizable compound may have one or more photocurable functional groups. The photocurable functional group in the cyclopolymerizable compound may be a group that does not undergo cyclopolymerization, or the photocurable functional group in the cyclopolymerizable compound may be a group that is not included in a ring structure after cyclization (a group that does not form a ring structure after cyclization). When the cyclopolymerizable compound has a photocurable functional group, the cyclopolymerizable compound may have one photocurable functional group, two photocurable functional groups, two or more photocurable functional groups, three or more photocurable functional groups, four or more photocurable functional groups, or five or more photocurable functional groups. The cyclopolymerizable compound may have 10 or less photocurable functional groups. From the viewpoint of more effectively exerting the effects of the present invention, it is preferable that the cyclopolymerizable compound includes a photocurable compound having one photocurable functional group. From the viewpoints of further enhancing the photocurability of the inkjet composition, favorably forming partition walls having a larger aspect ratio, increasing the glass transition temperature (Tg) of a cured product of the inkjet composition, and further enhancing the thermal cycling properties of the cured product of the inkjet composition, it is preferable that the cyclopolymerizable compound includes a photocurable compound having two or more photocurable functional groups.

[0076] Examples of the cyclopolymerizable group, the group containing the cyclopolymerizable group, or the photocurable functional group include a (meth)acryloyl group, an α-(allyloxymethyl)acryloyl group, and a vinyl group.

[0077] From the viewpoint of enhancing cyclopolymerizability, the cyclopolymerizable group or the group containing the cyclopolymerizable group of the cyclopolymerizable compound is preferably a (meth)acryloyl group or an α-(allyloxymethyl)acryloyl group. From the viewpoint of enhancing photocurability of the inkjet composition, the photocurable functional group of the cyclopolymerizable compound is preferably a (meth)acryloyl group or an α-(allyloxymethyl)acryloyl group. From the viewpoint of enhancing cyclopolymerizability and photocurability, the cyclopolymerizable compound preferably has a (meth)acryloyl group or an α-(allyloxymethyl)acryloyl group.

[0078] The cyclopolymerizable compound may have one (meth)acryloyl group or α-(allyloxymethyl)acryloyl group, two (meth)acryloyl groups or α-(allyloxymethyl)acryloyl groups, or two or more (meth)acryloyl groups or α-(allyloxymethyl)acryloyl groups. The cyclopolymerizable compound may have three or more (meth)acryloyl groups or α-(allyloxymethyl)acryloyl groups, four or more (meth)acryloyl groups or α-(allyloxymethyl)acryloyl groups, or five or more (meth)acryloyl groups or α-(allyloxymethyl)acryloyl groups. The cyclopolymerizable compound may have 10 or less (meth)acryloyl groups or α-(allyloxymethyl)acryloyl groups.

[0079] The cyclopolymerizable compound may be a monofunctional (meth)acrylate or a monofunctional α-(allyloxymethyl)acrylic acid, or may be a polyfunctional (meth)acrylate or a polyfunctional α-(allyloxymethyl)acrylic acid. From the viewpoints of further improving the cyclopolymerizability, further improving the photocurability, and favorably forming partition walls with a larger aspect ratio, the cyclopolymerizable compound preferably contains a polyfunctional (meth)acrylate or a polyfunctional α-(allyloxymethyl)acrylic acid. The cyclopolymerizable compound may contain a bifunctional (meth)acrylate compound or a bifunctional α-(allyloxymethyl)acrylic acid, or may contain a trifunctional (meth)acrylate compound or a trifunctional α-(allyloxymethyl)acrylic acid. The cyclopolymerizable compound may contain a tetrafunctional (meth)acrylate compound or a tetrafunctional α-(allyloxymethyl)acrylic acid, or may contain a pentafunctional (meth)acrylate compound or a pentafunctional α-(allyloxymethyl)acrylic acid. The cyclopolymerizable compound may contain a hexafunctional (meth)acrylate compound or a hexafunctional α-(allyloxymethyl)acrylic acid, or may contain a heptafunctional or higher functional (meth)acrylate compound or a heptafunctional or higher functional α-(allyloxymethyl)acrylic acid. The cyclopolymerizable compound may contain a decafunctional or lower functional (meth)acrylate compound or a decafunctional or lower functional α-(allyloxymethyl)acrylic acid.

[0080] Examples of the monofunctional (meth)acrylate or monofunctional α-(allyloxymethyl)acrylic acid include methyl-2-(allyloxymethyl)acrylic acid, 2-methoxyethyl-2-(allyloxymethyl)acrylic acid, tetrahydrofuran-2-ylmethyl-2-(allyloxymethyl)acrylic acid, 2-phenoxyethyl-2-(allyloxymethyl)acrylic acid, cyclohexyl-2-(allyloxymethyl)acrylic acid, and isobornyl-2-(allyloxymethyl)acrylic acid.

[0081] Examples of the difunctional (meth)acrylate or difunctional α-(allyloxymethyl)acrylic acid include tripropylene glycol di-2-(allyloxymethyl)acrylic acid, 1,6-hexanediol di-2-(allyloxymethyl)acrylic acid, neopentyl glycol di-2-(allyloxymethyl)acrylic acid, and tricyclodecane dimethanol di-2-(allyloxymethyl)acrylic acid.

[0082] Examples of the trifunctional (meth)acrylate or trifunctional α-(allyloxymethyl)acrylic acid include trimethylolpropane tri-2-(allyloxymethyl)acrylic acid.

[0083] Examples of the hexafunctional (meth)acrylate or hexafunctional α-(allyloxymethyl)acrylic acid include dipentaerythritol hexa-2-(allyloxymethyl)acrylic acid.

[0084] From the viewpoint of more effectively exerting the effects of the present invention, the cyclopolymerizable compound preferably has two or more carbon-carbon double bonds, and may have 12 or less, 8 or less, or 6 or less carbon-carbon double bonds.

[0085] From the viewpoint of more effectively exhibiting the effects of the present invention, the cyclopolymerizable compound preferably has an allyl ether group. From the viewpoint of more effectively exhibiting the effects of the present invention, the cyclopolymerizable group in the cyclopolymerizable compound is preferably an allyl ether group.

[0086] The cyclopolymerizable group or the group containing the cyclopolymerizable group is preferably a vinyl group, a (meth)acryloyl group, or an α-(allyloxymethyl)acryloyl group, and more preferably a (meth)acryloyl group or an α-(allyloxymethyl)acryloyl group. The photocurable functional group is preferably a vinyl group, a (meth)acryloyl group, or an α-(allyloxymethyl)acryloyl group, and more preferably a (meth)acryloyl group or an α-(allyloxymethyl)acryloyl group. The cyclopolymerizable compound preferably has a vinyl group, a (meth)acryloyl group, or an α-(allyloxymethyl)acryloyl group, and more preferably a (meth)acryloyl group or an α-(allyloxymethyl)acryloyl group. In these cases, partition walls having an even larger aspect ratio can be successfully formed, and the temperature-heat cycle characteristics of the cured product of the inkjet composition can be further improved, and reflow resistance can be further increased.

[0087] In order to more effectively exert the effects of the present invention, the cyclopolymerizable compound preferably has a structure represented by the following formula (1).

[0088]

[0089] In formula (1), R represents an organic group having 1 to 200 carbon atoms.

[0090] When the cyclopolymerizable compound has a structure represented by formula (1), the cyclopolymerizable compound can form a polymer having a five-membered cyclic ether structure in the main chain by radical polymerization.

[0091] In the above formula (1), the number of carbon atoms in R is 1 or more and 200 or less, preferably 150 or less, and more preferably 100 or less. In the above formula (1), R is preferably an alkyl group. In the above formula (1), R may be a linear alkyl group, a branched alkyl group, or a cyclic alkyl group. In the above formula (1), R may contain an ether bond.

[0092] In the above formula (1), examples of R include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, a tert-butyl group, an isobutyl group, a phenyl group, a pentyl group, a vinyl group, an allyl group, a crotyl group, a cyclopropyl group, a cyclobutyl group, a cyclohexyl group, a tetrahydrofurfuryl group, a methoxymethyl group, a methoxyethyl group, an ethoxymethyl group, an ethoxyethyl group, a phenoxyethyl group, a vinyloxyethyl group, an epoxy group, an isobornyl group, an adamantyl group, a dicyclopentadienyl group, and an oxetanyl group.

[0093] From the viewpoint of ejecting the ink jet composition satisfactorily using an ink jet device, in the above formula (1), R is preferably a methyl group or an ethyl group, and more preferably a methyl group.

[0094] The cyclopolymerizable compound may have an alicyclic skeleton. The cyclopolymerizable compound may be a cyclopolymerizable compound having an alicyclic skeleton. The cyclopolymerizable compound may have a cyclopolymerizable group and an alicyclic skeleton.

[0095] Examples of the cyclopolymerizable compound having an alicyclic skeleton include cyclohexyl-2-(allyloxymethyl)acrylic acid, isobornyl-2-(allyloxymethyl)acrylic acid, and tricyclodecane dimethanol di-2-(allyloxymethyl)acrylic acid.

[0096] In order to more effectively exert the effects of the present invention, the cyclopolymerizable compound preferably contains methyl-2-(allyloxymethyl)acrylic acid (that is, methyl 2-(allyloxymethyl)acrylate).

[0097] The photo- and thermosetting compound has a photo-curable functional group and a thermosetting functional group. Examples of the thermosetting functional group include a cyclic ether group, a maleimide group, and a cyclic thioether group. Examples of the cyclic ether group include an epoxy group and an oxetanyl group. The epoxy group may be an epoxy group in a glycidyl group. Examples of the cyclic thioether group include a thietane group and a thiirane group.

[0098] Examples of the photo- and thermosetting compounds include glycidyl (meth)acrylate, allyl glycidyl ether, 4-hydroxybutyl (meth)acrylate glycidyl ether, and 3,4-epoxycyclohexylmethyl (meth)acrylate.

[0099] The glass transition temperature (Tg) of the homopolymer of the (A) photocurable compound is preferably 100°C or higher, more preferably 130°C or higher, and even more preferably 160°C or higher. When the glass transition temperature (Tg) of the homopolymer of the (A) photocurable compound is equal to or higher than the lower limit, the thermal cycle properties can be further improved. The upper limit of the glass transition temperature (Tg) of the homopolymer of the (A) photocurable compound is not particularly limited. The glass transition temperature (Tg) of the homopolymer of the (A) photocurable compound may be 250°C or lower, or may be 220°C or lower. The range of the glass transition temperature (Tg) of the homopolymer of the (A) photocurable compound can be set by appropriately selecting the lower limit and the upper limit.

[0100] The glass transition temperature of the homopolymer of the photocurable compound (A) means the glass transition temperature of a homopolymer having a degree of polymerization of 3,000 to 4,000 (preferably 3,500).

[0101] The glass transition temperature can be measured using a differential scanning calorimeter at a temperature rise rate of 10°C / min in accordance with JIS K 7121. Examples of the differential scanning calorimeter include "DSC7020" manufactured by Hitachi High-Tech Science Corporation.

[0102]

[0044] The content of the photocurable compound (A) in 100% by weight of the ink jet composition is preferably 30% by weight or more, more preferably 40% by weight or more, even more preferably 60% by weight or more, and is preferably 75% by weight or less, more preferably 70% by weight or less, even more preferably 65% ​​by weight or less. When the content of the photocurable compound is equal to or more than the above lower limit and equal to or less than the above upper limit, partition walls having an even larger aspect ratio can be formed.

[0103] <(B) Thermosetting Compound> The (B) thermosetting compound does not have a photocurable functional group but has a thermosetting functional group.

[0104] Examples of the thermosetting functional group include a cyclic ether group, a maleimide group, and a cyclic thioether group. Examples of the cyclic ether group include an epoxy group and an oxetanyl group. The epoxy group may be an epoxy group in a glycidyl group. Examples of the cyclic thioether group include a thietane group and a thiirane group.

[0105] Examples of the (B) thermosetting compound include a compound having a cyclic ether group, a compound having a maleimide group, and a compound having a thiirane group. The (B) thermosetting compound may be used alone or in combination of two or more.

[0106] The thermosetting compound (B) is liquid at 25°C.

[0107] If the (B) thermosetting compound is solid at 25°C, it may be difficult to dissolve the (E) antioxidant in the inkjet composition, and the effects of the present invention may not be achieved. On the other hand, if the (B) thermosetting compound is liquid at 25°C, the (E) antioxidant described below can be sufficiently dissolved in the inkjet composition. As a result, the cooling / heating cycle characteristics can be improved, and when a reflective film is formed on the inner wall surface of the partition wall formed using the inkjet composition, the adhesion between the partition wall and the reflective film can be improved. Furthermore, if the (B) thermosetting compound is liquid at 25°C, the solubility of the (B) thermosetting compound in the inkjet composition is excellent, and therefore storage stability can be further improved.

[0108] The viscosity of the (B) thermosetting compound at 25° C. is preferably 100 mPa·s or more, more preferably 500 mPa·s or more, even more preferably 1000 mPa·s or more, and is preferably 70000 mPa·s or less, more preferably 30000 mPa·s or less, even more preferably 15000 mPa·s or less. When the (B) thermosetting compound has a viscosity at 25° C. that is equal to or more than the above lower limit and equal to or less than the above upper limit, the inkjet ejection properties are further improved, and the effects of the present invention can be exhibited more effectively.

[0109] The viscosity of the thermosetting compound (B) at 25°C is preferably measured using an E-type viscometer (for example, "TVE22L" manufactured by Toki Sangyo Co., Ltd.) under conditions of 25°C and 10 rpm.

[0110] From the viewpoint of enhancing thermosetting properties, the thermosetting compound (B) preferably has a cyclic ether group or a thiirane group, more preferably has a cyclic ether group or a cyclic thioether group, further preferably has a cyclic ether group, and particularly preferably has an epoxy group. From the viewpoint of enhancing thermosetting properties, the thermosetting compound (B) preferably contains an epoxy compound.

[0111] Examples of the epoxy compound include bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, bisphenol S type epoxy compounds, phenol novolac type epoxy compounds, cresol novolac type epoxy compounds, biphenyl type epoxy compounds, biphenyl novolac type epoxy compounds, biphenol type epoxy compounds, naphthalene type epoxy compounds, fluorene type epoxy compounds, phenol aralkyl type epoxy compounds, naphthol aralkyl type epoxy compounds, dicyclopentadiene type epoxy compounds, anthracene type epoxy compounds, epoxy compounds having an adamantane skeleton, epoxy compounds having a tricyclodecane skeleton, naphthylene ether type epoxy compounds, and epoxy compounds having a triazine nucleus in the skeleton.

[0112] From the viewpoint of more effectively exerting the effects of the present invention, the thermosetting compound (B) preferably contains an epoxy compound having an aromatic skeleton, and more preferably contains a bisphenol A epoxy compound or a bisphenol F epoxy compound. When the thermosetting compound (B) contains a bisphenol A epoxy compound or a bisphenol F epoxy compound, the reflow resistance can be further improved and the thermal cycle characteristics can be further improved.

[0113]

[0044] The content of the thermosetting compound (B) in 100 wt% of the inkjet composition is preferably 7 wt% or more, more preferably 10 wt% or more, even more preferably 15 wt% or more, and is preferably 40 wt% or less, more preferably 35 wt% or less, and even more preferably 30 wt% or less. When the content of the thermosetting compound (B) is equal to or more than the above lower limit and equal to or less than the above upper limit, the effects of the present invention are more effectively exhibited, the storage stability of the inkjet composition is improved, and partition walls having an even larger aspect ratio can be formed.

[0114]

[0044] The total content of the (A) photocurable compound and the (B) thermosetting compound, relative to 100% by weight of the inkjet composition, is preferably 70% by weight or more, more preferably 80% by weight or more, even more preferably 85% by weight or more, and is preferably 98% by weight or less, more preferably 95% by weight or less, and even more preferably 92% by weight or less. When the total content of the (A) photocurable compound and the (B) thermosetting compound is equal to or more than the above lower limit and equal to or less than the above upper limit, the effects of the present invention are more effectively exhibited, the storage stability of the inkjet composition is improved, and partition walls having an even larger aspect ratio can be formed.

[0115] <(C) Photopolymerization Initiator> The inkjet composition contains (C) a photopolymerization initiator.

[0116] Examples of the (C) photopolymerization initiator include a photoradical polymerization initiator and a photocationic polymerization initiator. The (C) photopolymerization initiator may be used alone or in combination of two or more.

[0117] The photoradical polymerization initiator is a compound that generates radicals upon irradiation with light and initiates a radical polymerization reaction. Examples of the photoradical polymerization initiator include benzoin-based photopolymerization initiators such as benzoin, benzoin methyl ether, benzoin ethyl ether, and benzoin isopropyl ether; alkylphenone-based photopolymerization initiators such as 2-hydroxy-2-methyl-1-phenyl-propan-1-one; acetophenone-based photopolymerization initiators such as acetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, and 1,1-dichloroacetophenone; 2- Methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1,2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, N,N-dimethylaminoacetophenone, 2-(dimethylamino)-2-( Aminoacetophenone-based photopolymerization initiators such as 4-methylbenzyl-1-(4-morpholinophenyl)butan-1-one and 2-methyl-[4-(methylthio)phenyl]-2-morpholino-1-propane; hydroxyacetophenones such as 1-hydroxycyclohexyl phenyl ketone; anthraquinone-based photopolymerization initiators such as 2-methylanthraquinone, 2-ethylanthraquinone, and 2-t-butylanthraquinone; 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone thioxanthone-based photopolymerization initiators such as 2-chlorothioxanthone and 2,4-diisopropylthioxanthone; ketal-based photopolymerization initiators such as acetophenone dimethyl ketal and benzil dimethyl ketal; acylphosphine oxide-based photopolymerization initiators such as 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide;Examples of suitable photopolymerization initiators include oxime ester photopolymerization initiators such as 1,2-octanedione, 1-[4-(phenylthio)-2-(o-benzoyloxime)], ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-1-(o-acetyloxime), and o-benzoyl-α-oxo oxime; and titanocene photopolymerization initiators such as bis(cyclopentadienyl)-di-phenyl-titanium, bis(cyclopentadienyl)-di-chloro-titanium, bis(cyclopentadienyl)-bis(2,3,4,5,6-pentafluorophenyl)titanium, and bis(cyclopentadienyl)-bis(2,6-difluoro-3-(pyrrol-1-yl)phenyl)titanium. The photoradical polymerization initiators may be used alone or in combination of two or more.

[0118] A photopolymerization initiation aid may be used together with the above-mentioned photoradical polymerization initiator. Examples of the photopolymerization initiation aid include N,N-dimethylaminobenzoic acid ethyl ester, N,N-dimethylaminobenzoic acid isoamyl ester, pentyl-4-dimethylaminobenzoate, triethylamine, and triethanolamine. Photopolymerization initiation aids other than these may also be used. The above-mentioned photopolymerization initiation aids may be used alone or in combination of two or more.

[0119] Examples of the photocationic polymerization initiator include sulfonium salts, iodonium salts, metallocene compounds, benzoin tosylate, etc. The photocationic polymerization initiator may be used alone or in combination of two or more.

[0120] From the viewpoint of forming partition walls having a larger aspect ratio, the (C) photopolymerization initiator preferably contains a photoradical polymerization initiator, more preferably contains an α-hydroxyacetophenone-based photopolymerization initiator, and further preferably contains an aminoacetophenone-based photopolymerization initiator. From the viewpoint of forming partition walls having a larger aspect ratio, the (C) photopolymerization initiator particularly preferably contains 2-(dimethylamino)-2-(4-methylbenzyl)-1-(4-morpholinophenyl)butan-1-one.

[0121]

[0044] The content of the photopolymerization initiator (C) relative to 100% by weight of the inkjet composition is preferably 0.1% by weight or more, more preferably 0.5% by weight or more, even more preferably 1% by weight or more, and is preferably 30% by weight or less, more preferably 20% by weight or less, even more preferably 10% by weight or less. When the content of the photopolymerization initiator (C) is equal to or more than the above lower limit and equal to or less than the above upper limit, partition walls having an even larger aspect ratio can be formed.

[0122] The content of the (C) photopolymerization initiator relative to 100 parts by weight of the (A) photocurable compound is preferably 1 part by weight or more, more preferably 3 parts by weight or more, even more preferably 5 parts by weight or more, and is preferably 30 parts by weight or less, more preferably 20 parts by weight or less, even more preferably 15 parts by weight or less. When the content of the (C) photopolymerization initiator is equal to or more than the above lower limit and equal to or less than the above upper limit, partition walls having an even larger aspect ratio can be formed.

[0123] <(D) Heat Curing Agent> The ink jet composition contains a (D) heat curing agent, which thermally cures the thermosetting compound.

[0124] Examples of the (D) heat curing agent include organic acids, amine compounds, amide compounds, hydrazide compounds, imidazole compounds, imidazoline compounds, phenol compounds, urea compounds, polysulfide compounds, and acid anhydrides. The (D) heat curing agent may be used alone or in combination of two or more.

[0125] Examples of the amine compound include aliphatic polyamines, alicyclic polyamines, aromatic polyamines, hydrazides, and guanidine derivatives. The amine compound may be a modified polyamine compound such as an amine-epoxy adduct. The amine compound may also be an adduct of the amine compound. Examples of the adduct of the amine compound include epoxy compound-added polyamines (reaction products of epoxy compounds and polyamines), Michael addition polyamines (reaction products of α,β-unsaturated ketones and polyamines), Mannich addition polyamines (condensates of polyamines with formalin and phenols), thiourea-added polyamines (reaction products of thiourea and polyamines), and ketone-blocked polyamines (reaction products (ketimines) of ketone compounds and polyamines).

[0126] Examples of the aliphatic polyamine include diethylenetriamine, triethylenetetramine, tetraethylenepentamine, and diethylaminopropylamine.

[0127] Examples of the alicyclic polyamine include menthene diamine, isophorone diamine, N-aminoethylpiperazine, 3,9-bis(3-aminopropyl)-2,4,8,10-tetraoxaspiro(5,5)undecane adduct, bis(4-amino-3-methylcyclohexyl)methane, and bis(4-aminocyclohexyl)methane.

[0128] Examples of the aromatic polyamine include m-phenylenediamine, p-phenylenediamine, o-xylylenediamine, m-xylylenediamine, p-xylylenediamine, 4,4-diaminodiphenylmethane, 4,4'-diamino-3,3'-diethyl-5,5'-dimethyldiphenylmethane, 4,4-diaminodiphenylpropane, 4,4-diaminodiphenylsulfone, 4,4-diaminodicyclohexane, bis(4-aminophenyl)phenylmethane, 1,5-diaminonaphthalene, 1,1-bis(4-aminophenyl)cyclohexane, 2,2-bis[(4-aminophenoxy)phenyl]propane, bis[4-(3-aminophenoxy)phenyl]sulfone, 1,3-bis(3-aminophenoxy)benzene, 4,4-methylene-bis(2-chloroaniline), and 4,4-diaminodiphenylsulfone.

[0129] Examples of the hydrazide include carbodihydrazide, adipic acid dihydrazide, sebacic acid dihydrazide, dodecanedioic acid dihydrazide, and isophthalic acid dihydrazide.

[0130] Examples of the guanidine derivatives include dicyandiamide, 1-o-tolyldiguanide, α-2,5-dimethylguanide, α,ω-diphenyldiguanidide, α,α-bisguanylguanidinodiphenyl ether, p-chlorophenyldiguanide, α,α-hexamethylenebis[ω-(p-chlorophenol)]diguanide, phenyldiguanide oxalate, acetylguanidine, and diethylcyanoacetylguanidine.

[0131] Examples of the phenol compound include polyhydric phenol compounds, such as phenol, cresol, ethylphenol, butylphenol, octylphenol, bisphenol A, tetrabromobisphenol A, bisphenol F, bisphenol S, 4,4′-biphenylphenol, naphthalene skeleton-containing phenol novolac resins, xylylene skeleton-containing phenol novolac resins, dicyclopentadiene skeleton-containing phenol novolac resins, and fluorene skeleton-containing phenol novolac resins.

[0132] Examples of the acid anhydride include phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylnadic anhydride, dodecylsuccinic anhydride, chlorendic anhydride, pyromellitic anhydride, benzophenonetetracarboxylic anhydride, methylcyclohexenetetracarboxylic anhydride, trimellitic anhydride, and polyazelaic anhydride.

[0133] The (D) heat curing agent preferably contains an amine compound, more preferably contains an aromatic amine compound, further preferably contains an aromatic polyamine, and particularly preferably contains 1,3-bis(3-aminophenoxy)benzene or bis[4-(3-aminophenoxy)phenyl]sulfone. In this case, the storage stability of the inkjet composition is improved, and high adhesion between the substrate and the partition walls can be maintained even when cooling and heating are repeated.

[0134]

[0044] The content of the (D) heat curing agent in 100 wt% of the ink jet composition is preferably 1 wt% or more, more preferably 5 wt% or more, even more preferably 7 wt% or more, and is preferably 40 wt% or less, more preferably 30 wt% or less, and even more preferably 20 wt% or less. When the content of the (D) heat curing agent is equal to or more than the above lower limit and equal to or less than the above upper limit, partition walls having a larger aspect ratio are formed, and high adhesion between the substrate and the partition walls can be maintained even when cooling and heating are repeated.

[0135] The content of the (D) thermosetting agent relative to 100 parts by weight of the (B) thermosetting compound is preferably 10 parts by weight or more, more preferably 20 parts by weight or more, even more preferably 30 parts by weight or more, and is preferably 110 parts by weight or less, more preferably 90 parts by weight or less, and even more preferably 70 parts by weight or less. When the content of the (D) thermosetting agent is equal to or more than the above lower limit and equal to or less than the above upper limit, partition walls having a larger aspect ratio can be formed, and high adhesion between the substrate and the partition walls can be maintained even when cooling and heating are repeatedly performed.

[0136] <(E) Antioxidant> The inkjet composition contains an antioxidant (E). Because the inkjet composition contains the antioxidant (E), it can improve its thermal cycling properties. The reason why the thermal cycling properties can be improved is thought to be that radicals generated at high temperatures, which cause resin degradation, are trapped by the antioxidant (E), thereby suppressing resin degradation. Furthermore, because the inkjet composition contains the antioxidant (E), it can improve the adhesion between the partition walls and the reflective film when a reflective film is formed on the inner wall surface of the partition walls formed using the inkjet composition.

[0137] Examples of the (E) antioxidant include phenol-based antioxidants, thioether-based antioxidants, and phosphorus-based antioxidants. The phenol-based antioxidants are antioxidants having a phenol skeleton. The thioether-based antioxidants are antioxidants having a thioether skeleton. The phosphorus-based antioxidants are antioxidants containing a phosphorus atom. The (E) antioxidants may be used alone or in combination of two or more.

[0138] Examples of the phenolic antioxidant include 2,6-di-t-butyl-p-cresol (BHT), butylhydroxyanisole (BHA), 2,6-di-t-butyl-4-ethylphenol, stearyl-β-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 2,2'-methylenebis-(4-methyl-6-butylphenol), 2,2'-methylenebis-(4-ethyl-6-t-butylphenol), 4,4'-butylidene-bis-(3-methyl-6-t-butylphenol), 1,1,3-tris-(2-methyl-hydroxy-5-t 1,3,3-tris-(2-methyl-4-hydroxy-5-t-butylphenol)butane, tetrakis[methylene-3-(3',5'-butyl-4-hydroxyphenyl)propionate]methane, 1,3,3-tris-(2-methyl-4-hydroxy-5-t-butylphenol)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, bis(3,3'-t-butylphenol)butyric acid glycol ester, and bis(3-t-butyl-4-hydroxy-5-methylbenzenepropanoate)ethylenebis(oxyethylene).

[0139] Examples of the thioether antioxidant include distearyl thiodipropionate, pentaerythritol-tetrakis(dodecylthiopropionate), pentaerythritol-tetrakis(3-laurylthiopropionate), pentaerythritol-tetrakis(stearylthiopropionate), pentaerythritol-tetrakis(laurylthiobutyrate), pentaerythritol-tetrakis(myristylthiopropionate), and pentaerythritol-tetrakis(laurylthioacetate).

[0140] Examples of the phosphorus-based antioxidant include tridecyl phosphite, tris(tridecyl)phosphite, triphenyl phosphite, trinonylphenyl phosphite, bis(tridecyl)pentaerythritol diphosphite, bis(decyl)pentaerythritol diphosphite, tris(2,4-di-t-butylphenyl)phosphite, bis(2,4-di-t-butyl-6-methylphenyl)ethyl ester phosphorous acid, and 2,2′-methylenebis(4,6-di-t-butyl-1-phenyloxy)(2-ethylhexyloxy)phosphorus.

[0141] From the viewpoint of further improving the ink jet ejection properties and storage stability of the ink jet composition, the (E) antioxidant preferably contains a phenol-based antioxidant, and is more preferably a phenol-based antioxidant. From the viewpoint of further improving the ink jet ejection properties and storage stability of the ink jet composition, the (E) antioxidant preferably does not contain a thioether-based antioxidant, preferably does not contain a phosphorus-based antioxidant, and preferably does not contain an antioxidant other than a phenol-based antioxidant. The phenol-based antioxidant may be a hindered phenol-based antioxidant.

[0142]

[0043] The content of the antioxidant (E) in 100% by weight of the ink jet composition is preferably 0.1% by weight or more, more preferably 0.3% by weight or more, even more preferably 0.5% by weight or more, and is preferably 5% by weight or less, more preferably 4% by weight or less, and even more preferably 3% by weight or less. When the content of the antioxidant (E) is equal to or more than the above lower limit and equal to or less than the above upper limit, the effects of the present invention can be more effectively exhibited.

[0143]

[0044] The content of the phenolic antioxidant in the ink jet composition (100% by weight) is preferably 0.1% by weight or more, more preferably 0.3% by weight or more, even more preferably 0.5% by weight or more, and is preferably 5% by weight or less, more preferably 4% by weight or less, and even more preferably 3% by weight or less. When the content of the phenolic antioxidant is equal to or more than the above lower limit and equal to or less than the above upper limit, the effects of the present invention are more effectively exhibited, and the ink jet ejection properties of the ink jet composition can be further improved, and the storage stability can be increased.

[0144] The content of the (E) antioxidant relative to 100 parts by weight of the (B) thermosetting compound is preferably 1 part by weight or more, more preferably 1.5 parts by weight or more, even more preferably 3 parts by weight or more, and still more preferably 5 parts by weight or more, and is preferably 35 parts by weight or less, more preferably 30 parts by weight or less, and particularly preferably 15 parts by weight or less. When the content of the (E) antioxidant is not less than the above lower limit and not more than the above upper limit, the effects of the present invention can be more effectively exhibited.

[0145] The content of the phenolic antioxidant relative to 100 parts by weight of the (B) thermosetting compound is preferably at least 1 part by weight, more preferably at least 1.5 parts by weight, even more preferably at least 3 parts by weight, and particularly preferably at least 5 parts by weight, and is preferably at most 35 parts by weight, more preferably at most 20 parts by weight, and even more preferably at most 15 parts by weight. When the content of the phenolic antioxidant is at least the above-mentioned lower limit and at most the above-mentioned upper limit, the effects of the present invention can be more effectively exhibited.

[0146] <Other Components> The inkjet composition may contain other components in addition to the components described above. Examples of the other components include a coupling agent, a dispersant, a filler, a leveling agent, an antifoaming agent, a curing accelerator, a solvent, and a polymerization inhibitor.

[0147] The inkjet composition may contain colorants such as pigments and dyes as other components, but preferably does not contain a colorant. When the inkjet composition does not contain a colorant, the photoreactivity can be further improved, and the effects of the present invention can be more effectively exhibited. The colorants such as pigments and dyes are not particularly limited, but examples thereof include black colorants such as carbon black.

[0148] (LED module and manufacturing method of LED module) The LED module according to the present invention comprises a substrate, an LED chip arranged on a first surface of the substrate, and a partition wall arranged on the first surface of the substrate. In the LED module, the partition wall is arranged on the first surface of the substrate so as to surround the LED chip. In the LED module, the partition wall is a cured product of the above-mentioned inkjet composition for forming a partition wall.

[0149] The LED module according to the present invention has the above-described configuration, and therefore can improve reflow resistance and thermal cycle characteristics.

[0150] The LED module according to the present invention preferably further comprises a reflective film on the inner wall surface of the partition wall.

[0151] The method for manufacturing an LED module according to the present invention uses an electronic component including a substrate and an LED chip arranged on a first surface of the substrate. The method for manufacturing an LED module according to the present invention comprises the following steps: applying the above-mentioned inkjet composition for partition wall formation onto the first surface of the substrate in the electronic component by inkjet printing to form an inkjet composition layer; and curing the inkjet composition layer to form a partition wall on the first surface of the substrate. In the method for manufacturing an LED module according to the present invention, in the obtained LED module, the partition wall is arranged on the first surface of the substrate so as to surround the LED chip, and the partition wall is a cured product of the inkjet composition for partition wall formation.

[0152] The method for manufacturing an LED module according to the present invention has the above-described configuration, and therefore can improve reflow resistance and thermal cycle characteristics.

[0153] The method for manufacturing an LED module according to the present invention preferably includes the step of arranging the LED chip on the first surface of the substrate to obtain an electronic component.

[0154] The method for manufacturing an LED module according to the present invention preferably includes the step of arranging a reflective film on the inner wall surface of the partition wall.

[0155] Specific embodiments of the present invention will be described below with reference to the drawings. Note that in the drawings, the size, thickness, shape, etc. may differ from the actual size, thickness, shape, etc. for the sake of convenience of illustration.

[0156] Fig. 1(a) is a plan view schematically showing an LED module obtained using the ink jet composition for partition wall formation according to the first embodiment of the present invention. Fig. 1(b) is a cross-sectional view schematically showing the LED module. Fig. 1(b) is a cross-sectional view taken along line II in Fig. 1(a).

[0157] The LED module 1 shown in FIG. 1 includes a substrate 11, an LED chip 12 disposed on a first surface 11a of the substrate 11, and a partition wall 13 disposed on the first surface 11a of the substrate 11. In the LED module 1, the partition wall 13 is disposed on the first surface 11a of the substrate 11 so as to surround the LED chip 12. In the LED module 1, the partition wall 13 is a cured product of the inkjet composition for partition wall formation described above. An interval is provided between the outer surface of the LED chip 12 and the inner surface of the partition wall 13. A space exists between the outer surface of the LED chip 12 and the inner surface of the partition wall 13. In the LED module 1, the partition wall 13 is formed from the inkjet composition for partition wall formation described above. The partition wall 13 is not disposed (formed) on the surface of the LED chip 12. The upper surface of the LED chip 12 is not covered by the partition wall 13. The partition wall 13 has a frame-like shape.

[0158] FIG. 2 is a cross-sectional view schematically showing an LED module obtained using an ink jet composition for forming a partition wall according to a second embodiment of the present invention.

[0159] The LED module 1A shown in FIG. 2 further includes a reflective film 14 on the inner wall surface (inner surface) of the partition wall 13. There is a gap between the outer surface of the LED chip 12 and the inner surface of the partition wall 13. There is a gap between the outer surface of the LED chip 12 and the inner surface of the partition wall 13. There is a gap between the outer surface of the LED chip 12 and the inner surface of the reflective film 14. There is a gap between the outer surface of the LED chip 12 and the inner surface of the reflective film 14. The LED module 1A differs from the LED module 1 only in the reflective film 14. The LED module may or may not further include a reflective film on the inner wall surface of the partition wall.

[0160] In the LED module according to the present invention, the partition wall is preferably arranged in a frame shape. In the LED module, the partition wall is preferably not arranged in the center of the substrate. From the viewpoint of increasing brightness of the LED module, it is preferable that an outer surface of the LED chip and an inner surface of the partition wall are spaced apart. From the viewpoint of increasing brightness of the LED module, it is preferable that a space exists between the outer surface of the LED chip and the inner surface of the partition wall.

[0161] The width, height, etc. of the partition wall can be changed as appropriate.

[0162] The width of the partition wall may be 30 μm or more, 50 μm or more, or 70 μm or more, or may be 1000 μm or less, 800 μm or less, or 700 μm or less.

[0163] From the viewpoint of further increasing the extraction efficiency of light generated from the LED chip, the height of the LED chip is preferably 10 μm or more, more preferably 20 μm or more, even more preferably 50 μm or more, and is preferably 300 μm or less, more preferably 200 μm or less, even more preferably 150 μm or less.

[0164] From the viewpoint of further increasing the extraction efficiency of light generated from the LED chip, the height of the partition wall is preferably 100 μm or more, more preferably 300 μm or more, even more preferably 600 μm or more, and is preferably 3000 μm or less, more preferably 2000 μm or less, even more preferably 1500 μm or less.

[0165] From the viewpoint of further increasing the extraction efficiency of light generated from the LED chip, the height of the partition is preferably at least 50 μm higher than the height of the LED chip, more preferably at least 100 μm higher, and even more preferably at least 200 μm higher.

[0166] The aspect ratio (ratio of height to width (height / width)) of the partition wall is preferably 5 or more, more preferably 8 or more, and further preferably 10 or more. The aspect ratio (ratio of height to width (height / width)) of the partition wall may be 100 or less, 50 or less, 25 or less, or 15 or less.

[0167] The substrate may be a transparent material or may not be a transparent material. Examples of the substrate include a circuit board and a silicon substrate.

[0168] The LED chip may be a red LED chip, a blue LED chip, a green LED chip, a UV-LED chip, or a combination of these LED chips. The UV-LED chip may be a deep ultraviolet UV-LED chip.

[0169] The LED module may or may not further include a reflective film on the inner wall surface of the partition wall. From the viewpoint of further increasing the extraction efficiency of light generated from the LED chip, the LED module preferably further includes a reflective film on the inner wall surface of the partition wall. The manufacturing method for the LED module preferably includes a step of arranging a reflective film on the inner wall surface of the partition wall. The reflective film may or may not be formed on the outer wall surface of the partition wall. When a reflective film is provided on the inner wall surface of the partition wall, the LED module can improve adhesion between the partition wall and the reflective film. More specifically, when a reflective film is provided on the inner wall surface of the partition wall, the LED module can prevent the reflective film from peeling off from the partition wall even when heated by reflow.

[0170] Examples of the material for the reflective film include silver, chromium, copper, titanium, and aluminum. Only one material for the reflective film may be used, or two or more materials may be used in combination. From the viewpoint of further increasing the utilization efficiency of light generated from the LED chip, the material for the reflective film is preferably titanium or aluminum.

[0171] Examples of methods for forming the reflective film on the inner wall surface of the partition wall include electroless plating, electroplating, physical collision, mechanochemical reaction, physical film formation, physical adsorption, and a method of coating the surface of the partition wall with a metal powder or a paste containing a metal powder and a binder. The method for forming the reflective film on the surface of the partition wall is preferably electroless plating, electroplating, or a physical collision method. Examples of the physical film formation method include vacuum deposition, ion plating, and ion sputtering. Furthermore, the physical collision method uses a sheeter composer (manufactured by Tokuju Kosakusho Co., Ltd.) or the like.

[0172] The shape of the LED module is not particularly limited, and may be round, rectangular, or triangular.

[0173] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0174] The following materials were prepared:

[0175] (A) Photocurable compounds: Trifunctional (meth)acrylate compound: trimethylolpropane triacrylate ("TMPTA" manufactured by Daicel-Allnex Corporation, glass transition temperature of homopolymer: 180°C) Bifunctional (meth)acrylate compound 1: tricyclodecane dimethanol diacrylate ("IRR214K" manufactured by Daicel-Allnex Corporation, (meth)acrylate compound having a dicyclopentadiene skeleton, glass transition temperature of homopolymer: 190°C) Bifunctional (meth)acrylate compound 2: 1,6-hexanediol diacrylate ("HDDA" manufactured by Daicel-Allnex Corporation, glass transition temperature of homopolymer: 105°C) Bifunctional (meth)acrylate compound 3: dipropylene glycol diacrylate ("DPGDA" manufactured by Daicel-Allnex Corporation, glass transition temperature of homopolymer: 110°C) Bifunctional (meth)acrylate compound 4: ethoxylated bisphenol A diacrylate ("APG700" manufactured by Shin-Nakamura Chemical Co., Ltd., glass transition temperature of homopolymer: 65°C) Bifunctional (meth)acrylate compound 5: 1,9-nonanediol diacrylate ("1,9-NDDA" manufactured by Osaka Organic Chemical Industry Ltd., glass transition temperature of homopolymer: 100°C) Monofunctional (meth)acrylate compound: 2-ethylhexyl acrylate ("2EHA" manufactured by Nippon Shokubai Co., Ltd., glass transition temperature of homopolymer: -30°C) Half ester (photo- and thermosetting compound): 4-hydroxybutyl (meth)acrylate glycidyl ether ("4HBAGE" manufactured by Mitsubishi Chemical Corporation, glass transition temperature of homopolymer: -60°C)

[0176] (B) Thermosetting compounds: Epoxy compound 1: bisphenol A type epoxy compound (DIC Corporation "CRP850", viscosity at 25°C 4500 mPa·s (liquid at 25°C)) Epoxy compound 2: bisphenol F type epoxy compound (DIC Corporation "CRP830", viscosity at 25°C 1300 mPa·s (liquid at 25°C)) Epoxy compound 3: dicyclopentadiene dimethanol diglycidyl ether (ADEKA Corporation "EP4088S", viscosity at 25°C 230 mPa·s (liquid at 25°C)) Epoxy compound 4: bisphenol A type epoxy compound (Nippon Steel Chemical & Material Co., Ltd. "YD127", viscosity at 25°C 9500 mPa·s (liquid at 25°C)) Epoxy compound 5: dicyclopentadiene-type epoxy compound ("HP7200L" manufactured by DIC Corporation, solid at 25°C)

[0177] (C) Photopolymerization initiator: 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone (Irgacure 379, manufactured by IGM)

[0178] (D) Heat curing agent: 1,3-bis(3-aminophenoxy)benzene ("APB-N" manufactured by Mitsui Chemicals, Inc.), 4,4'-diamino-3,3'-diethyl-5,5'-dimethyldiphenylmethane ("Curehard MED-J" manufactured by Kumiai Chemical Industry Co., Ltd.), dimethylthiotoluenediamine ("EH-105L" manufactured by ADEKA Corporation).

[0179] (E) Antioxidants: Phenol-based antioxidant 1 ("ADEKA STAB AO-60" manufactured by ADEKA Corporation) Phenol-based antioxidant 2 ("ADEKA STAB AO-80" manufactured by ADEKA Corporation) Thioether-based antioxidant ("ADEKA STAB AO-503" manufactured by ADEKA Corporation) Phosphorus-based antioxidant ("ADEKA STAB PEP-36" manufactured by ADEKA Corporation)

[0180] Curing accelerator: DBU-octylate ("UCAT SA102" manufactured by San-Apro Co., Ltd.)

[0181] Polymerization inhibitor: copper(II) dibutyldithiocarbamate ("TBT-Cu" manufactured by Sanshin Chemical Industry Co., Ltd.)

[0182] Coupling agent: 3-glycidoxypropyltriethoxysilane ("KBE-403" manufactured by Shin-Etsu Chemical Co., Ltd.)

[0183] (Examples 1 to 15 and Comparative Examples 1 to 4) Preparation of inkjet compositions: The components shown in Tables 1 to 5 were blended in the blending amounts (% by weight) shown in Tables 1 to 5 and mixed uniformly to obtain inkjet compositions for forming partition walls (inkjet compositions).

[0184] Formation of partition walls: An aluminum nitride substrate having a surface roughness Ra of 0.4 μm was prepared. The ink jet composition obtained was applied onto the surface of the substrate while circulating at 75° C., and a first light irradiation step (UV-LED lamp with a dominant wavelength of 365 nm, 4000 mW / cm 2 This process was repeated for 0.1 seconds after application to form a B-staged product having a width of 600 μm, a length of 5 mm, and a height of 1000 μm. Thereafter, a second light irradiation process (metal halide lamp, 1000 mW / cm 2 The curing was then allowed to proceed by irradiation with light for 10 seconds. Thereafter, the substrate was heated at 200° C. for 1 hour for thermal curing, thereby obtaining a laminate in which partition walls were formed on the surface of the substrate.

[0185] (Evaluation) (1) Storage Stability (1-1) Storage The obtained inkjet composition was stored at −20° C. and 5° C. for 48 hours, respectively, and then filtered using a 0.2 μm membrane filter to observe whether or not a precipitate was present. The storage stability (storage) was evaluated according to the following criteria.

[0186] [Criteria for storage stability (keeping)] ◯: No precipitate at both -20°C and 5°C ○: Precipitation at either -20°C or 5°C ×: Precipitation at both -20°C and 5°C

[0187] (1-2) High Temperature In accordance with JIS K2283, the viscosity (η1) of the obtained inkjet composition was measured at 5 rpm at a temperature at which the viscosity became 20 mPa s using an E-type viscometer ("TVE22L" manufactured by Toki Sangyo Co., Ltd.). In addition, after heating for 12 hours at a temperature at which the viscosity of the inkjet composition became 20 mPa s, the viscosity (η2) was measured at 5 rpm at the same temperature. The ratio (η2 / η1) of the viscosity (η2) to the viscosity (η1) was calculated. The storage stability (high temperature) was evaluated according to the following criteria.

[0188] [Criteria for storage stability (high temperature)] ○○: The ratio (η2 / η1) is 1.0 or more and less than 1.1. ○: The ratio (η2 / η1) is 1.1 or more and less than 1.2. ×: The ratio (η2 / η1) is 1.2 or more.

[0189] (2) Formability of Partition Walls with a Large Aspect Ratio The resulting inkjet composition was applied to a substrate using an inkjet head of a piezoelectric inkjet printer equipped with an ultraviolet irradiation device. The applied inkjet composition was then irradiated with ultraviolet light to form a B-staged material layer. The above application and photocuring steps were repeated in the thickness direction of the formed B-staged material layer. The resulting B-staged material layer was then heated and thermally cured to form partition walls. The shapes of the resulting partition walls were observed using a laser microscope (Olympus Corporation, "OLS4100") to confirm whether or not partition walls with a width of 1) 300 μm and a height of 1000 μm, 2) 200 μm and a height of 1000 μm, and 3) 100 μm and a height of 1000 μm could be formed. The formability of partition walls with a large aspect ratio was evaluated according to the following criteria.

[0190] [Criteria for determining the formability of barrier ribs with a large aspect ratio] ◯: All barrier ribs 1), 2), and 3) could be formed. ○: The barrier rib 1) could not be formed, but the barrier ribs 2) and 3) could be formed. Δ: The barrier ribs 1) and 2) could not be formed, but the barrier rib 3) could be formed. ×: All barrier ribs 1), 2), and 3) could not be formed.

[0191] (3) Reflow Resistance (3-1) Mechanical Strength of Partition Walls (Initial) The obtained laminate was subjected to a reflow treatment for 3 minutes (30 seconds at a peak top temperature of 320°C). The laminate after the reflow treatment was observed using a microscope (Keyence Corporation's "VHX-5000") to determine whether the partition walls had peeled off from the substrate and whether cracks had occurred in the partition walls. Furthermore, the die shear strength of the laminate before and after the reflow treatment was measured using a die shear strength measuring device (Nordson Corporation's "DAGE 4000PXY") by pressing the partition walls at a height of 500 μm from the substrate surface under conditions of a blade length of 2 mm and a speed of 10 μm / s. The die shear strength before the reflow treatment was defined as F1, and the die shear strength after the reflow treatment was defined as F2, and the ratio (F2 / F1) was calculated. The mechanical strength (initial) of the partition walls was evaluated according to the following criteria.

[0192] [Evaluation criteria for partition wall mechanical strength (initial)] ◯: No separation or cracking of the partition walls occurred, and the ratio (F2 / F1) was 0.90 or more. ○: No separation or cracking of the partition walls occurred, but the ratio (F2 / F1) was 0.80 or more and less than 0.90. ×: Separation or cracking of the partition walls occurred, or the ratio (F2 / F1) was less than 0.80.

[0193] (3-2) Adhesion between Substrate and Partition Wall (Initial) The obtained laminate was subjected to a reflow treatment for 3 minutes (30 seconds at a peak top temperature of 320°C). After the reflow treatment, the laminate was subjected to a die shear strength F3 measurement by pressing the partition wall at a height of 125 μm from the substrate surface using a die shear strength measurement device (Nordson "DAGE 4000PXY") under conditions of a blade length of 2 mm and a speed of 10 μm / s. The adhesion between the substrate and partition wall (initial) was evaluated according to the following criteria.

[0194] [Criteria for determining (initial) adhesion between substrate and partition wall] ○○: F3 is 40N or more ○: F3 is 30N or more but less than 40N ×: F3 is less than 30N

[0195] (4) Thermal Cycle Characteristics (4-1) Mechanical Strength of Partition Walls (Long Term) The laminate after the reflow treatment was subjected to a thermal cycle of cooling at -40°C for 15 minutes, heating to 125°C at a heating rate of 10°C / min, heating at 125°C for 15 minutes, and cooling to -40°C at a cooling rate of 10°C / min, which was repeated 1,000 times. The die shear strength F4 of the laminate after the thermal cycle test was measured by pressing the partition walls at a height of 500 μm from the substrate surface using a die shear strength measuring device (Nordson "DAGE 4000PXY") under conditions of a blade length of 2 mm and a speed of 150 μm / s. The mechanical strength (long term) of the partition walls was evaluated according to the following criteria.

[0196] [Criteria for determining mechanical strength (long-term) of partition walls] ○○: F4 is 3 kg or more ○: F4 is 2 kg or more but less than 3 kg ×: F4 is less than 2 kg

[0197] (4-2) Adhesion between Substrate and Partition Wall (Long Term) For the laminate after the above-mentioned thermal cycle test, the die shear strength F5 was measured by pressing the partition wall at a height of 125 μm from the substrate surface using a die shear strength measuring device (Nordson "DAGE 4000PXY") under conditions of a blade length of 2 mm and a speed of 10 μm / s, and the ratio (F5 / F3) was calculated. The adhesion (long term) between the substrate and the partition wall was evaluated according to the following criteria.

[0198] [Criteria for determining (long-term) adhesion between substrate and partition wall] ◯: Ratio (F5 / F3) is 0.90 or more ○: Ratio (F5 / F3) is 0.80 or more and less than 0.90 ×: Ratio (F5 / F3) is less than 0.80

[0199] (5) Adhesion between the partition wall and the reflective film (sputtering characteristics) The obtained laminate was subjected to a sputtering process using a sputtering module (Q150T ES manufactured by Quorum Technologies) with a 5×10 -3A titanium film was formed to a thickness of 100 nm by sputtering at 100 Pa, and an aluminum film was further formed thereon to a thickness of 500 nm, thereby forming a reflective film on the surface of the partition wall. The sputtered laminate was subjected to a reflow treatment for 3 minutes (30 seconds at a peak top temperature of 320°C). The reflective film on the surface of the partition wall of the laminate after the reflow treatment was observed using a microscope (Keyence Corporation, "VHX-5000"). The adhesion between the partition wall and the reflective film was evaluated according to the following criteria.

[0200] [Criteria for determining adhesion between partition wall and reflective film] ◯: Peeling or cracking of the reflective film did not occur. ×: Peeling or cracking of the reflective film occurred.

[0201] The compositions and results are shown in Tables 1 to 5 below.

[0202]

[0203]

[0204]

[0205]

[0206]

[0207] REFERENCE SIGNS LIST 1, 1A... LED module 11... substrate 11a... first surface 12... LED chip 13... partition wall 14... reflective film

Claims

1. An inkjet composition for forming a partition wall, comprising: a photocurable compound having a photocurable functional group and either a thermosetting functional group or not; a thermosetting compound having either a photocurable functional group or not and a thermosetting functional group; a photopolymerization initiator; a heat curing agent; and an antioxidant, wherein the thermosetting compound is liquid at 25°C.

2. The ink jet composition for forming partition walls according to claim 1, wherein the antioxidant comprises a phenol-based antioxidant.

3. The ink jet composition for forming partition walls according to claim 1 or 2, wherein the thermosetting compound contains a bisphenol A type epoxy compound or a bisphenol F type epoxy compound.

4. The ink jet composition for forming partition walls according to any one of claims 1 to 3, wherein the photocurable compound contains a photocurable compound having two or more (meth)acryloyl groups and having an alicyclic skeleton.

5. The ink jet composition for forming partition walls according to any one of claims 1 to 4, wherein the photocurable compound contains a photocurable compound having two or more (meth)acryloyl groups and having a dicyclopentadiene skeleton.

6. The ink jet composition for forming a partition wall according to any one of claims 1 to 5, wherein the content of the photocurable compound is 40% by weight or more and 75% by weight or less in 100% by weight of the ink jet composition for forming a partition wall.

7. The ink jet composition for forming a partition wall according to any one of claims 1 to 6, wherein the content of the thermosetting compound is 10% by weight or more and 35% by weight or less in 100% by weight of the ink jet composition for forming a partition wall.

8. The ink jet composition for forming a partition wall according to any one of claims 1 to 7, wherein the content of the antioxidant is 0.3% by weight or more and 4% by weight or less, based on 100% by weight of the ink jet composition for forming a partition wall.

9. The ink jet composition for forming a partition wall according to any one of claims 1 to 8, wherein the photopolymerization initiator includes an aminoacetophenone-based photopolymerization initiator.

10. The ink jet composition for forming partition walls according to any one of claims 1 to 9, wherein the heat curing agent contains an aromatic amine compound.

11. The ink jet composition for forming partition walls according to any one of claims 1 to 10, wherein the heat curing agent contains 1,3-bis(3-aminophenoxy)benzene or bis[4-(3-aminophenoxy)phenyl]sulfone.

12. An LED module comprising: a substrate; an LED chip arranged on a first surface of the substrate; and a partition arranged on the first surface of the substrate, the partition being arranged on the first surface of the substrate so as to surround the LED chip, and the partition being a cured product of the inkjet composition for forming a partition according to any one of claims 1 to 11.

13. The LED module according to claim 12, further comprising a reflective film on an inner wall surface of the partition.

14. A method for manufacturing an LED module, comprising the steps of: using an electronic component comprising a substrate and an LED chip disposed on a first surface of the substrate, applying the partition-forming inkjet composition according to any one of claims 1 to 11 onto the first surface of the substrate in the electronic component by an inkjet method to form an inkjet composition layer; and curing the inkjet composition layer to form a partition on the first surface of the substrate, wherein in the resulting LED module, the partition is disposed on the first surface of the substrate so as to surround the LED chip, and the partition is a cured product of the partition-forming inkjet composition.

15. The method for manufacturing an LED module according to claim 14, further comprising the step of arranging a reflective film on the inner wall surface of the partition wall.

Citation Information

Patent Citations

  • Method of resotring partition wall, restored partition wall and optical element

    JP2020182948A

  • Micro LED display unit

    JP2020205417A

  • Liquid-repellent curable ink composition

    WO2013024764A1

  • Curable composition for inkjet and for partition wall formation, light-emitting device, and method for manufacturing light-emitting device

    WO2022260049A1