Water-soluble film, medicine packaging body using same, and methods for producing these
The combination of gelatin and modified polyvinyl alcohol resin in a water-soluble film addresses the mechanical and sealing weaknesses of conventional films, providing enhanced strength and solubility for effective drug and food packaging while maintaining biodegradability.
Patent Information
- Application Number
- PCT/JP2024/011808
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional gelatin-containing films lack sufficient mechanical properties, such as strength and elongation, and sealing performance, particularly when packaging liquids, leading to concerns about liquid leakage and inadequate durability.
A water-soluble film composed of gelatin and modified polyvinyl alcohol resin, which enhances compatibility, mechanical properties, and sealing performance while maintaining biodegradability, is developed. The film includes a modified polyvinyl alcohol resin with anionic groups, carboxy groups, or sulfonic acid groups, and a plasticizer, with a water content of 3 to 15% by mass, suitable for drug packaging.
The film exhibits excellent water solubility, mechanical strength, and sealing properties, reducing the risk of liquid leakage and maintaining solubility over time, making it suitable for individual packaging of medicines and foods without compromising biodegradability.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Water-soluble film, drug package using same, and manufacturing method thereof
[0001] The present invention relates to a water-soluble film containing gelatin, which is a naturally occurring raw material, and more particularly to a water-soluble film containing gelatin and a polyvinyl alcohol-based resin, and a pharmaceutical package using the same.
[0002] Water-soluble films using gelatin, a naturally occurring raw material, have been known as packaging materials for foods, etc. For example, an edible film excellent in solubility, heat-sealability, and blocking properties is produced by mixing pectin, glycerin, and a sucrose fatty acid ester with a gelatin base and molding the mixture into a film (see Patent Document 1), and a packaging film made of a material containing a small amount of collagen added to gelatin, which prevents the contents from absorbing moisture or releasing flavors, aromas, and other components during storage, and which dissolves in hot water when used (see Patent Document 2).
[0003] Other proposed films include an edible film with improved moisture resistance and heat sealing properties, which has a hydrophobic layer of food-grade wax or the like formed on one side of an edible base film formed by mixing agar and gelatin (see Patent Document 3), and an edible film with excellent heat solubility, heat sealing properties, and processability, which contains a binder containing at least inulin and other binders such as agar, carrageenan, gelatin, furcellaran, pectin, etc. (see Patent Document 4).
[0004] Furthermore, in recent years, from the perspective of protecting the global environment, there is a growing expectation for the development of highly biodegradable films made from natural materials to replace the conventional plastic films made from petroleum-derived materials. Gelatin, which is primarily composed of protein, is attracting attention as an alternative to petroleum-derived materials and as a raw material for packaging films from the standpoints of safety, price, etc.
[0005] Japanese Patent Laid-Open No. 6-105660 Japanese Patent Laid-Open No. 6-183456 Japanese Patent Laid-Open No. 2002-95426 Japanese Patent Laid-Open No. 2008-79525
[0006] However, the above-mentioned conventional gelatin-containing films do not have sufficient mechanical properties such as strength and elongation, and further improvements are required to make them stronger and more moldable, particularly for use in individual packaging of foods, medicines, etc. Furthermore, with regard to sealing properties, particularly when packaging liquids, there is a concern of liquid leakage if the strength of the sealed portion is low, and further improvements are required.
[0007] Therefore, in this context, the present invention provides a water-soluble film that is a gelatin-containing film that has excellent water solubility and mechanical properties such as film strength and elongation, as well as excellent sealing properties, a pharmaceutical packaging body using the same, and methods for manufacturing the same.
[0008] However, the present inventors have conducted extensive research in light of these circumstances and have found that by using a modified polyvinyl alcohol resin as a material to be used in combination with gelatin, a water-soluble film can be obtained that has excellent compatibility with gelatin and is excellent in water solubility, mechanical properties, and sealability. Because polyvinyl alcohol resins are biodegradable resins, it is possible to solve the above problems without significantly reducing the biodegradability of the water-soluble film as a whole, and it is also possible to reduce the proportion of petroleum-derived raw materials compared to water-soluble films made of conventional polyvinyl alcohol resins.
[0009] That is, the present invention has the following aspects. [1] A water-soluble film containing gelatin and a polyvinyl alcohol-based resin (A), wherein the polyvinyl alcohol-based resin (A) contains a modified polyvinyl alcohol-based resin. [2] The water-soluble film according to [1], wherein the modified polyvinyl alcohol-based resin contains at least one modified polyvinyl alcohol-based resin selected from the group consisting of anionic group-modified polyvinyl alcohol, pyrrolidone ring group-modified polyvinyl alcohol, and amino group-modified polyvinyl alcohol. [3] The water-soluble film according to [1] or [2], further containing a plasticizer. [4] The water-soluble film according to any one of [1] to [3], which has a water content of 3 to 15% by mass. [5] The water-soluble film according to any one of [1] to [4], which is used for packaging medicines. [6] The water-soluble film according to any one of [1] to [5], wherein the increase in the dissolution time of the film is less than 70% when the film is left in static contact for three weeks in a mixed solution of 11.2% by mass of propylene glycol, 13.4% by mass of glycerin, 8.4% by mass of ethanolamine, and 11.8% by mass of water, pH 9.5. [7] The water-soluble film according to any one of [1] to [6], wherein the increase in the dissolution time of the film is less than 70% when the film is left in static contact for three weeks in a mixed solution of 6.2% by mass of propylene glycol, 10.9% by mass of glycerin, 7.6% by mass of ethanolamine, and 12.5% by mass of water, pH 7.0. [8] A pharmaceutical package comprising a package made of the water-soluble film according to any one of [1] to [7] and a pharmaceutical packaged in the package. [9] The pharmaceutical package according to [8], wherein the pharmaceutical is a liquid detergent.
[10] The pharmaceutical package according to [9], wherein the liquid detergent has a pH of 6 to 9 when dissolved or dispersed in water.
[11] A method for producing the water-soluble film according to any one of [1] to [7], comprising: a casting step of preparing a film-forming raw material containing gelatin and a modified polyvinyl alcohol-based resin; and a drying step of drying the cast film-forming raw material.
[12] A method for producing a drug package described in any one of [8] to
[10] , comprising the steps of preparing a first water-soluble film, a second water-soluble film, and a drug, placing the first water-soluble film and the second water-soluble film opposite each other with the drug interposed between them, and partially abutting the first water-soluble film and the second water-soluble film, and crimping the abutting portion between the first water-soluble film and the second water-soluble film.
[0010] The water-soluble film of the present invention has high compatibility with gelatin and modified polyvinyl alcohol-based resins, excellent water solubility (solubility), and excellent mechanical properties and sealing properties. Furthermore, when used as a package, the film solubility is prevented from decreasing over time. Therefore, the film is suitable for packaging applications, and is particularly excellent as an individual package for medicines and foods.
[0011] The present invention will be described below based on examples of embodiments for carrying out the present invention, but the present invention is not limited to the embodiments described below.
[0012] Furthermore, in this specification, when the expression "X to Y" (X and Y are any numbers) is used, unless otherwise specified, it means "X or more and Y or less," as well as "preferably greater than X" or "preferably smaller than Y." Furthermore, when the expression "X or more" (X is any number) or "Y or less" (Y is any number) is used, it also means "preferably greater than X" or "preferably less than Y." Furthermore, "x and / or y (x and y are any configurations)" means at least one of x and y, and can mean three possibilities: x only, y only, or x and y. For numerical ranges described in stages in this specification, the upper or lower limit of a numerical range in one stage can be arbitrarily combined with the upper or lower limit of a numerical range in another stage. Furthermore, in the numerical ranges described in this specification, the upper or lower limit of the numerical range can also be replaced with the values shown in the examples. In this specification, the term "main component" means a component that has a significant effect on the properties of the target object, and the content of the component is usually 50% by mass or more, preferably 55% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more, and may be 100% by mass.
[0013] In the present invention, the term "water-soluble film" refers to a film that dissolves in water at about room temperature (20°C). In the present invention, the solubility of a film is determined as follows: a film is cut into a size of 3 cm x 5 cm, placed in a 1-liter beaker containing 1 liter of water and fixed with a jig, and stirred with a stirrer (rotor length 3 cm, rotation speed 750 rpm) while maintaining the water temperature at 20°C. Dissolution is determined when no insoluble fine particles of the film with a diameter of 1 mm or more are observed.
[0014] A water-soluble film according to one embodiment of the present invention (hereinafter sometimes referred to as "the present water-soluble film") contains gelatin and a polyvinyl alcohol-based resin (A). A drug package according to one embodiment of the present invention comprises a package made of the water-soluble film and a drug contained in the package. These will be explained below. In the present invention, polyvinyl alcohol may be abbreviated as "PVA." The term "film" also encompasses "tape" and "sheet."
[0015] <Gelatin> Gelatin is extracted from collagen, the main component of the bones and skin of animals such as cows and pigs, and is chemically composed primarily of a linear polymer (protein) of amino acids. It is generally used as a food additive as a gelling agent or thickener.
[0016] Typically, an aqueous gelatin solution gels at temperatures below 25°C and dissolves at temperatures above 30°C. Gelatin is classified into two types, acid-treated and alkali-treated, depending on the manufacturing method, and each has a different isoelectric point. While the isoelectric point of acid-treated gelatin is a wide range from 6 to 9, the isoelectric point of alkali-treated gelatin is a narrow range around 5. Normally, using gelatin at a pH near its isoelectric point leads to a decrease in gel strength and turbidity of the gel.
[0017] In the water-soluble film of the present invention, it is preferable to use alkali-treated gelatin because it has excellent physical properties.
[0018] <PVA-Based Resin (A)> The PVA-based resin (A) may be used alone, or may contain two or more PVA-based resins that differ in at least one of the degree of saponification, viscosity, modified species, and modification amount.
[0019] In the water-soluble film of the present invention, the PVA-based resin (A) contains a modified PVA-based resin as an essential component. The modified PVA-based resin preferably accounts for 50% by mass or more of the PVA-based resin (A), more preferably 55% by mass or more, even more preferably 60% by mass or more, particularly preferably 70% by mass or more, and may even account for 100% by mass.
[0020] Specific preferred examples of the PVA-based resin (A) containing a modified PVA-based resin include a resin containing one kind of modified PVA-based resin, a resin containing two or more kinds of modified PVA-based resins, and a resin containing two or more kinds of modified PVA-based resins in combination with unmodified PVA. Of these, a resin containing only one kind of modified PVA-based resin or a resin containing a modified PVA-based resin in combination with unmodified PVA is preferred.
[0021] The mass content ratio of the modified PVA-based resin to the unmodified PVA, i.e., modified PVA-based resin / unmodified PVA, is preferably from 100 / 0 to 50 / 50, particularly preferably from 100 / 0 to 55 / 45. From the viewpoint of film properties such as water solubility and water sealability, the mass content ratio is preferably from 99 / 1 to 55 / 45, particularly preferably from 95 / 5 to 60 / 40, and further preferably from 90 / 10 to 70 / 30.
[0022] The modified PVA-based resin used in the present water-soluble film is preferably a modified PVA-based resin having at least one modifying group selected from an anionic group such as a carboxy group, a sulfonic acid group, or a phosphate group, a pyrrolidone ring group, or an amino group, from the viewpoints of compatibility with gelatin and solubility of the film. Among these, an anionic group-modified PVA-based resin is preferably used, and examples of the anionic group include a carboxy group, a sulfonic acid group, and a phosphate group. From the viewpoint of stability of solubility over time, a carboxy group or a sulfonic acid group is preferred, and a carboxy group-modified PVA-based resin is particularly preferred.
[0023] The average saponification degree of the PVA-based resin (A) is preferably 80 mol% or more, particularly preferably 82 to 99.9 mol%, further preferably 85 to 98 mol%, and particularly preferably 90 to 96 mol%. If the average saponification degree is too low, the solubility of the film in water tends to decrease, or the solubility of the film tends to decrease over time depending on the packaging material. However, if the average saponification degree is too high, the solubility in water tends to decrease.
[0024] When unmodified PVA is used as the PVA-based resin (A), the average saponification degree of the unmodified PVA is preferably 80 mol% or more, particularly preferably 82 to 99 mol%, and even more preferably 85 to 90 mol%. If the average saponification degree is too low, the solubility of the water-soluble film in water tends to decrease. However, if the average saponification degree is too high, the solubility in water tends to decrease.
[0025] The average saponification degree of the PVA-based resin (A) means that the average saponification degree of the entire PVA-based resin contained in the present water-soluble film is within these ranges.
[0026] When a modified PVA-based resin is used as the PVA-based resin (A), the average saponification degree of the modified PVA-based resin is preferably 80 mol% or more, particularly preferably 85 to 99.9 mol%, and even more preferably 90 to 99 mol%. If the average saponification degree is too low, the solubility of the water-soluble film in water tends to decrease over time depending on the pH of the drug to be packaged. If the average saponification degree is too high, the solubility of the water-soluble film in water tends to decrease significantly due to the thermal history during film formation.
[0027] When an anionic group-modified PVA-based resin is used as the modified PVA-based resin, the average saponification degree thereof is preferably 85 to 99.9 mol%, particularly preferably 88 to 98 mol%, further preferably 90 to 97 mol%, and particularly preferably 90 to 95 mol%.
[0028] The viscosity of a 4% by mass aqueous solution of the PVA-based resin (A) at 20° C. is preferably 5 to 60 mPa s, particularly preferably 10 to 45 mPa s, further preferably 15 to 40 mPa s, and particularly preferably 21 to 35 mPa s. If the viscosity is too low, the mechanical strength of the water-soluble film tends to decrease, whereas if the viscosity is too high, the viscosity of the aqueous solution during film formation tends to increase, resulting in decreased productivity.
[0029] The viscosity of a 4% by mass aqueous solution of the PVA-based resin (A) at 20°C means that the viscosity of a 4% by mass aqueous solution of the entire PVA-based resin contained in the water-soluble film at 20°C falls within these ranges.
[0030] When an unmodified PVA is used as the PVA-based resin (A), the viscosity of a 4% by mass aqueous solution of the unmodified PVA at 20° C. is preferably 10 to 60 mPa s, particularly preferably 20 to 50 mPa s, and further preferably 30 to 45 mPa s. If the viscosity is too low, the mechanical strength of the water-soluble film used as a packaging material tends to decrease, whereas if the viscosity is too high, the viscosity of the aqueous solution during film formation tends to be high, resulting in decreased productivity.
[0031] When a modified PVA-based resin is used as the PVA-based resin (A), the viscosity of a 4% by mass aqueous solution of the modified PVA-based resin at 20° C. is preferably 5 to 50 mPa s, particularly preferably 10 to 40 mPa s, and further preferably 15 to 35 mPa s. If the viscosity is too low, the mechanical strength of the water-soluble film used as a packaging material tends to decrease, whereas if the viscosity is too high, the viscosity of the aqueous solution during film formation tends to be high, resulting in decreased productivity.
[0032] The modification amount of the PVA resin (A) is preferably 1 to 20 mol %, more preferably 1.5 to 15 mol %, and particularly preferably 2 to 12 mol %. If the modification amount is too small, the solubility of the water-soluble film in water tends to decrease, while if the modification amount is too large, the productivity of the PVA resin tends to decrease, the biodegradability tends to decrease, and the water-soluble film tends to be prone to blocking.
[0033] When an anionic group-modified PVA-based resin is used as the modified PVA-based resin, the modification amount of the anionic group-modified PVA-based resin is preferably 1 to 10 mol %, more preferably 1.5 to 9 mol %, and particularly preferably 2 to 8 mol %. If the modification amount is too small, the solubility of the water-soluble film in water tends to decrease, while if the modification amount is too large, the productivity of the PVA resin tends to decrease, the biodegradability tends to decrease, and the water-soluble film tends to be prone to blocking.
[0034] The average degree of saponification is measured in accordance with JIS K 6726 3.5, and the viscosity of a 4% by mass aqueous solution is measured in accordance with JIS K 6726 3.11.2.
[0035] The unmodified PVA can be produced by saponifying a polyvinyl ester resin obtained by polymerizing a vinyl ester compound.
[0036] Examples of such vinyl ester compounds include vinyl formate, vinyl acetate, vinyl trifluoroacetate, vinyl propionate, vinyl butyrate, vinyl caprate, vinyl laurate, vinyl versatate, vinyl palmitate, vinyl stearate, etc., with vinyl acetate being preferred. The above vinyl ester compounds may be used alone or in combination of two or more.
[0037] As a method for polymerizing the vinyl ester compound, any known polymerization method can be used, such as solution polymerization, emulsion polymerization, suspension polymerization, etc., but the vinyl ester compound is usually polymerized by a solution polymerization method using an alcohol such as methanol, ethanol, or isopropyl alcohol as a solvent.
[0038] The polymerization catalyst can be appropriately selected from known polymerization catalysts depending on the polymerization method, such as azo catalysts such as azobisisobutyronitrile, and peroxide catalysts such as acetyl peroxide, benzoyl peroxide, lauroyl peroxide, etc. The polymerization reaction temperature is selected from the range of 50°C to about the boiling point.
[0039] The saponification can be carried out by a known method, and is usually carried out by dissolving the obtained copolymer in alcohol in the presence of a saponification catalyst. Examples of alcohol include methanol, ethanol, and butanol. The concentration of the copolymer in the alcohol is selected from the range of 20 to 50% by mass in terms of solubility.
[0040] As the saponification catalyst, for example, an alkali catalyst such as an alkali metal hydroxide or alcoholate, such as sodium hydroxide, potassium hydroxide, sodium methylate, sodium ethylate, or potassium methylate, can be used, or an acid catalyst can also be used. The amount of the saponification catalyst used is preferably 1 to 100 millimole equivalents relative to the vinyl ester compound.
[0041] The modified PVA resin can be produced, for example, by saponifying a copolymer of a vinyl ester compound and an unsaturated monomer, or by post-modifying unmodified PVA.
[0042] As such a vinyl ester compound, the same compounds as those used in the case of the unmodified PVA can be used.
[0043] Examples of unsaturated monomers copolymerized with vinyl ester monomers for use in copolymerized modified PVA-based resins (copolymerized modified PVA-based resins) include olefins such as ethylene, propylene, isobutylene, α-octene, α-dodecene, and α-octadecene; hydroxyl-containing α-olefins such as 3-buten-1-ol, 4-penten-1-ol, and 5-hexen-1-ol, and derivatives thereof such as acylated products; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, maleic anhydride, itaconic acid, and undecylenic acid, as well as their salts, monoesters, and dialkyl esters; amides such as diacetone acrylamide, acrylamide, and methacrylamide; olefin sulfonic acids such as ethylene sulfonic acid, allyl sulfonic acid, and methallylsulfonic acid, as well as their salts; and N-vinyl pyrrolidone. These may be used alone or in combination of two or more.
[0044] Examples of PVA-based resins modified by a post-reaction (post-modified PVA-based resins) include those having an acetoacetyl group by reaction with diketene, those having a polyalkylene oxide group by reaction with ethylene oxide, those having a hydroxyalkyl group by reaction with an epoxy compound or the like, and those obtained by reacting an aldehyde compound or the like having various functional groups with a PVA-based resin by esterification, acetalization, urethanization, etherification, grafting, phosphate esterification, oxyalkylenation, or the like.
[0045] The modified PVA-based resin also includes a resin having primary hydroxyl groups in the side chain, typically 1 to 5, preferably 1 to 2, and particularly preferably 1 primary hydroxyl group in the side chain. Furthermore, it is preferable that the resin has a secondary hydroxyl group in addition to the primary hydroxyl group. Examples of such modified PVA-based resins include a modified PVA-based resin having a hydroxyalkyl group in the side chain and a modified PVA-based resin having a 1,2-diol structural unit in the side chain. The modified PVA-based resin having a 1,2-diol structural unit in the side chain can be produced by, for example, (i) a method of saponifying a copolymer of vinyl acetate and 3,4-diacetoxy-1-butene, (ii) a method of saponifying and decarboxylating a copolymer of vinyl acetate and vinyl ethylene carbonate, (iii) a method of saponifying and deketalizing a copolymer of vinyl acetate and 2,2-dialkyl-4-vinyl-1,3-dioxolane, or (iv) a method of saponifying a copolymer of vinyl acetate and glycerin monoallyl ether.
[0046] The copolymerization method of the vinyl ester compound and the unsaturated monomer copolymerizable with the vinyl ester compound can be the same as that for the unmodified PVA, and is usually carried out by a solution polymerization method using an alcohol as a solvent. The polymerization catalyst, saponification method, saponification catalyst, etc. can also be appropriately selected from the same as those for the unmodified PVA.
[0047] The carboxyl group-modified PVA-based resin can be produced by any method, for example, (I) a method of copolymerizing an unsaturated monomer having a carboxyl group with a vinyl ester-based compound, followed by saponification, or (II) a method of polymerizing a vinyl ester-based compound in the presence of an alcohol, aldehyde, or thiol having a carboxyl group as a chain transfer agent, followed by saponification.
[0048] As the vinyl ester compound in the above method (I) or (II), the compounds mentioned above can be used, but it is preferable to use vinyl acetate.
[0049] Examples of the unsaturated monomer having a carboxy group in the above method (I) include ethylenically unsaturated dicarboxylic acids (maleic acid, fumaric acid, itaconic acid, etc.), ethylenically unsaturated dicarboxylic acid monoesters (maleic acid monoalkyl esters, fumaric acid monoalkyl esters, itaconic acid monoalkyl esters, etc.), ethylenically unsaturated dicarboxylic acid diesters (maleic acid dialkyl esters, fumaric acid dialkyl esters, itaconic acid dialkyl esters, etc.) (however, it is necessary that these diesters are converted to a carboxy group by hydrolysis during saponification of the copolymer), or ethylenically unsaturated carboxylic acid anhydrides (maleic anhydride, Examples of the monomer include monomers such as maleic anhydride (itaconic acid, crotonic acid, etc.) and ethylenically unsaturated monocarboxylic acids ((meth)acrylic acid, crotonic acid, etc.), and salts thereof. Among these, it is preferable to use maleic acid, maleic acid monoalkyl esters, maleic acid dialkyl esters, maleic acid salts, maleic anhydride, itaconic acid, itaconic acid monoalkyl esters, itaconic acid dialkyl esters, (meth)acrylic acid, etc., and it is further preferable to use maleic acid-based monomers such as maleic acid, maleic acid monoalkyl esters, maleic acid dialkyl esters, maleic acid salts, and maleic anhydride, and it is particularly preferable to use maleic acid monoalkyl esters. These can be used alone or in combination of two or more.
[0050] In the above method (II), it is preferable to use a chain transfer agent, and as the chain transfer agent, a thiol compound having a large chain transfer effect is usually preferred, and examples thereof include the following compounds and their salts. These can be used alone or in combination of two or more kinds:
[0051]
[0052]
[0053] [In the above general formulas (1) and (2), n is an integer of 0 to 5, and R 1 , R 2 , R 3 represents a hydrogen atom or a lower alkyl group (which may contain a substituent).
[0054]
[0055] [In the above general formula (3), n is an integer of 0 to 20.]
[0056] Specific examples include mercaptoacetic acid, 2-mercaptopropionic acid, 3-mercaptopropionic acid, and 2-mercaptostearic acid.
[0057] In addition to the unsaturated monomer having a carboxy group and the vinyl ester compound, other general monomers may be contained in the polymerization to the extent that water solubility is not impaired. Examples of such monomers that can be used include alkyl esters of ethylenically unsaturated carboxylic acids, allyl esters of saturated carboxylic acids, α-olefins, alkyl vinyl ethers, alkyl allyl ethers, (meth)acrylamide, (meth)acrylonitrile, styrene, vinyl chloride, and the like.
[0058] The method for producing the carboxyl group-modified PVA-based resin is not limited to the above-mentioned method. For example, a method of post-reacting polyvinyl alcohol (partially saponified or completely saponified) with a carboxyl group-containing compound having a functional group reactive with a hydroxyl group, such as a dicarboxylic acid, an aldehydecarboxylic acid, or a hydroxycarboxylic acid, can also be employed.
[0059] The sulfonic acid-modified PVA resin can be produced, for example, by a method in which a copolymerization component such as vinyl sulfonic acid, styrene sulfonic acid, allyl sulfonic acid, methallyl sulfonic acid, or 2-acrylamido-2-methylpropanesulfonic acid is copolymerized with a vinyl ester compound, followed by saponification; or by a method in which vinyl sulfonic acid or a salt thereof, 2-acrylamido-2-methylpropanesulfonic acid or a salt thereof, or the like is subjected to Michael addition to PVA.
[0060] From the viewpoint of film properties such as solubility and mechanical properties, the content of the PVA-based resin (A) in the water-soluble film is preferably 30% by mass or more, particularly preferably 35% by mass or more, and even more preferably 40% by mass or more. If the content is too low, the solubility in water and the mechanical properties of the film tend to decrease. The upper limit of the content is usually 85% by mass or less, preferably 80% by mass or less, particularly preferably 75% by mass or less, from the viewpoint of shape stability over time when used as a package.
[0061] The mass ratio of gelatin to PVA-based resin (A) is preferably 1 / 99 to 99 / 1, particularly preferably 5 / 95 to 80 / 20, further preferably 10 / 90 to 60 / 40, and particularly preferably 15 / 85 to 45 / 55. If the gelatin content is too high, compatibility with the PVA-based resin (A) tends to be poor, which may reduce the solubility of the film in water. Furthermore, mechanical properties such as film strength tend to be reduced.
[0062] <Plasticizer> In order to impart appropriate flexibility to the water-soluble film, it is preferable to use a plasticizer in addition to gelatin and the PVA-based resin (A). One type of plasticizer may be used alone, or two or more types may be used in combination. However, in terms of the mechanical properties and moldability of the film, it is also preferable to use two or more types in combination.
[0063] Examples of such plasticizers include glycerins such as glycerin, diglycerin, and triglycerin; alkylene glycols such as diethylene glycol, triethylene glycol, polyethylene glycol, propylene glycol, polypropylene glycol, and dipropylene glycol; and sugar alcohols such as trimethylolpropane, sorbitol, xylitol, and maltitol. These may be used alone or in combination of two or more. Among these, glycerin, diglycerin, and polyethylene glycol are preferred because they are easily available and can achieve a plasticizing effect with a small amount. In addition, sorbitol is preferred in terms of the stability of the package over time, and a combination of glycerin and sorbitol is also preferred.
[0064] The content of the plasticizer is preferably 10 to 60 parts by mass, particularly preferably 15 to 55 parts by mass, further preferably 18 to 50 parts by mass, and particularly preferably 20 to 45 parts by mass, per 100 parts by mass of the total of gelatin and PVA-based resin (A). If the content of such a plasticizer is too low, the plasticizing effect is low, resulting in a decrease in processability, and when used as a package, the toughness of the water-soluble film tends to be impaired over time. If the content of such a plasticizer is too high, the strength of the film tends to be reduced and blocking tends to occur easily.
[0065] <Filler> The water-soluble film may further contain a filler, if necessary. The filler is added for the purpose of enhancing blocking resistance. Such a filler is not particularly limited, and either an organic filler or an inorganic filler may be used, with organic fillers being particularly preferred. These may be used alone or in combination of two or more. The average particle size of the filler is preferably 0.1 to 50 μm, and particularly preferably 1 to 35 μm. The average particle size of the filler is a value measured using a laser diffraction particle size distribution analyzer, and is calculated from the D50 value (particle size at 50% of the cumulative volume) of the obtained cumulative volume distribution.
[0066] The organic filler refers to particulate matter (primary particles) composed of an organic compound and having any shape, such as needle-like, rod-like, layer-like, scale-like, or spherical, or an aggregate of such particulate matter (secondary particles). Such organic fillers are mainly selected from polymer compounds, and examples thereof include melamine-based resins, polymethyl (meth)acrylate-based resins, polystyrene-based resins, as well as biodegradable resins such as starch and polylactic acid. Among these, biodegradable resins such as polymethyl (meth)acrylate-based resins, polystyrene-based resins, and starch are preferred, and starch is particularly preferred in terms of dispersibility in the PVA-based resin (A).
[0067] Examples of the starch include raw starches (corn starch, potato starch, sweet potato starch, wheat starch, cassava starch, sago starch, tapioca starch, sorghum starch, rice starch, bean starch, kudzu starch, bracken starch, lotus starch, water chestnut starch, etc.), physically modified starches (α-starch, fractionated amylose, moist heat-treated starch, etc.), enzyme-modified starches (hydrolyzed dextrin, enzymatically decomposed dextrin, amylose, etc.), chemically decomposed modified starches (acid-treated starch, hypochlorite oxidized starch, dialdehyde starch, etc.), and chemically modified starch derivatives (esterified starch, etherified starch, cationized starch, cross-linked starch, etc.). Of these, raw starches, particularly corn starch and rice starch, are preferably used from the standpoints of availability and economy.
[0068] The average particle size of the organic filler is preferably 3 to 50 μm, particularly preferably 5 to 40 μm, and further preferably 10 to 35 μm. If the average particle size is too small, the blocking tendency of the film tends to increase, while if it is too large, the fillers tend to aggregate with each other, reducing dispersibility and causing pinholes when the film is stretched during molding.
[0069] The inorganic filler refers to particulate matter (primary particles) composed of an inorganic compound and having any shape, such as needle-like, rod-like, layer-like, scale-like, or spherical, or an aggregate of such particulate matter (secondary particles). Examples of inorganic fillers include oxide-based inorganic compounds such as silica (silicon dioxide), diatomaceous earth, titanium oxide, calcium oxide, magnesium oxide, aluminum oxide, barium oxide, germanium oxide, tin oxide, and zinc oxide, as well as talc, clay, kaolin, mica, asbestos, gypsum, graphite, glass balloons, glass beads, calcium sulfate, barium sulfate, ammonium sulfate, calcium sulfite, calcium carbonate, whisker-like calcium carbonate, magnesium carbonate, dawsonite, dolomite, potassium titanate, carbon black, glass fibers, alumina fibers, boron fibers, processed mineral fibers, carbon fibers, hollow carbon spheres, bentonite, montmorillonite, copper powder, sodium sulfate, potassium sulfate, zinc sulfate, copper sulfate, iron sulfate, magnesium sulfate, aluminum sulfate, potassium aluminum sulfate, ammonium nitrate, sodium nitrate, potassium nitrate, aluminum nitrate, ammonium chloride, sodium chloride, potassium chloride, magnesium chloride, calcium chloride, sodium phosphate, and potassium chromate. These may be used alone or in combination of two or more.
[0070] Among these, it is preferable to use silica, oxide-based inorganic compounds, and talc, and it is particularly preferable to use silica, titanium oxide, and talc, and it is further preferable to use silica.
[0071] The average particle size of the inorganic filler is preferably 1 to 20 μm, particularly preferably 2 to 15 μm, and further preferably 3 to 10 μm. If the average particle size is too small, the flexibility and toughness of the film tend to decrease and blocking tends to increase, while if the average particle size is too large, pinholes tend to form when the film is stretched during molding.
[0072] The content of the filler is preferably 1 to 30 parts by mass, particularly preferably 2 to 25 parts by mass, and even more preferably 2.5 to 20 parts by mass, per 100 parts by mass of gelatin and PVA-based resin (A). If the content is too low, blocking tends to increase, while if the content is too high, the flexibility and toughness of the film tend to decrease. From the viewpoint of the balance between the blocking resistance of the film and its mechanical properties and sealability, the content of the filler is preferably 12 parts by mass or less, particularly preferably 1 to 11 parts by mass, further preferably 2 to 10 parts by mass, and even more preferably 2.5 to 9 parts by mass, per 100 parts by mass of the PVA-based resin (A).
[0073] <Surfactant> The water-soluble film may further contain a surfactant, etc., if necessary. The surfactant is contained for the purpose of improving the releasability from the casting surface during film production, and typically includes a nonionic surfactant, a cationic surfactant, and an anionic surfactant. Examples of such surfactants include polyoxyethylene nonylphenyl ether, polyoxyethylene octylnonyl ether, polyoxyethylene dodecylphenyl ether, polyoxyethylene alkyl allyl ether, polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan monooleate, polyoxyalkylene alkyl ether phosphate ester monoethanolamine salt, polyoxyethylene lauryl amino ether, polyoxyethylene stearyl amino ether and other polyoxyethylene alkyl amino ethers, sorbitan monopalmitate, sorbitan monostearate, glycerol stearate, sucrose fatty acid ester, etc., and these may be used alone or in combination of two or more. Among these, polyoxyalkylene alkyl ether phosphate monoethanolamine salt and polyoxyethylene lauryl amino ether are preferred from the viewpoint of production stability. These surfactants may be used alone or in combination of two or more.
[0074] The content of the surfactant is preferably 0.01 to 3 parts by mass, particularly preferably 0.05 to 2.5 parts by mass, and even more preferably 0.1 to 2 parts by mass, per 100 parts by mass of the total of gelatin and PVA-based resin (A). If the content is too low, the peelability between the casting surface of the film-forming apparatus and the formed film tends to decrease, resulting in a decrease in productivity. If the content is too high, blocking tends to occur easily, and when the film is used to form a package, the adhesive strength at the time of sealing tends to decrease.
[0075] <Other Components> The water-soluble film of the present invention may contain other components, such as water-soluble polymers other than the PVA-based resin (A) (e.g., sodium polyacrylate, polyethylene oxide, polyvinylpyrrolidone, dextrin, chitosan, chitin, methylcellulose, hydroxyethyl cellulose, etc.), fragrances, rust inhibitors, colorants, bulking agents, antifoaming agents, ultraviolet absorbers, liquid paraffins, fluorescent brighteners, bitter components (e.g., denatonium benzoate, etc.), etc., within the scope of the invention. These may be used alone or in combination of two or more.
[0076] The content of the other components is preferably 5 parts by mass or less, particularly preferably 1 part by mass or less, and even more preferably 0.5 parts by mass or less, per 100 parts by mass of the PVA-based resin (A). The lower limit is usually 0 part by mass. If the content is too high, compatibility with gelatin decreases, and durability tends to decrease.
[0077] The water-soluble film may also contain an antioxidant. Examples of such antioxidants include sulfites such as sodium sulfite, potassium sulfite, calcium sulfite, and ammonium sulfite, as well as tartaric acid, ascorbic acid, sodium thiosulfate, techol, and Rongalit. Of these, sulfites, particularly sodium sulfite, are preferred. The amount of such antioxidant added is preferably 0.1 to 10 parts by mass, particularly preferably 0.2 to 5 parts by mass, and even more preferably 0.3 to 3 parts by mass, per 100 parts by mass of the PVA-based resin (A).
[0078] <<Production of Water-Soluble Film>> The present water-soluble film is produced by blending gelatin and the PVA-based resin (A), preferably further comprising a plasticizer, and optionally further comprising other components such as a filler and a surfactant, and dissolving or dispersing the blend in water to prepare a film-forming raw material, which is then formed into a film. The production of such a water-soluble film includes a casting step of casting the film-forming raw material onto a casting surface, and a drying step of drying the cast film-forming raw material.
[0079] <Dissolving Step> In the dissolving step, the above-mentioned blended components are dissolved or dispersed in water to prepare an aqueous solution or aqueous dispersion serving as a film-forming raw material. The method for mixing gelatin, PVA-based resin (A), and other additives in the preparation of the film-forming raw material is not particularly limited, and examples thereof include: (i) a method in which gelatin, PVA-based resin (A), and other additives are mixed to prepare a mixture, and the mixture is then mixed with water to dissolve, (ii) a method in which PVA-based resin (A) and other additives are dissolved in water, and then gelatin is mixed, (iii) a method in which gelatin, PVA-based resin (A), and other additives are separately dissolved in water, and then these are mixed, and (iv) a method in which gelatin and PVA-based resin (A) are separately dissolved in water, and then these are mixed with other additives to dissolve.
[0080] The dissolution method for dissolving in water typically includes room temperature dissolution, high temperature dissolution, and pressure dissolution. Among these, high temperature dissolution and pressure dissolution are preferred because they result in less undissolved material and are superior in productivity. The dissolution temperature for high temperature dissolution is typically 80 to 100°C, preferably 90 to 100°C, and for pressure dissolution, it is typically 80 to 130°C, preferably 90 to 120°C. In particular, the dissolution temperature for gelatin is preferably 50 to 90°C, particularly preferably 55 to 85°C, and more preferably 60 to 80°C. The dissolution time is typically 1 to 20 hours, preferably 2 to 15 hours, and more preferably 3 to 10 hours. If the dissolution time is too short, undissolved material tends to remain, while if it is too long, productivity tends to decrease.
[0081] Furthermore, after dissolution, the resulting film-forming raw material is subjected to a degassing treatment. Examples of such degassing methods include static degassing, vacuum degassing, and twin-screw extrusion degassing, with static degassing and twin-screw extrusion degassing being preferred. The degassing temperature is usually 50 to 100°C, preferably 55 to 95°C, and particularly preferably 60 to 80°C. If the degassing temperature is too high, proteins, which are components of gelatin, will denature, causing coloration and a decrease in strength. If the temperature is too low, the viscosity will increase, requiring a long time for degassing, which tends to reduce productivity. The degassing time is usually 2 to 30 hours, preferably 5 to 25 hours.
[0082] The solids concentration of the film-forming raw material is preferably 10 to 60% by mass, particularly preferably 12 to 50% by mass, and even more preferably 15 to 40% by mass. If the concentration is too low, film productivity tends to decrease, while if it is too high, the viscosity becomes too high, which tends to require a long time to degas the film-forming raw material and to cause die lines during film formation. The pH of the film-forming raw material is usually 4 to 8, preferably 4.8 to 7.5.
[0083] <Film-forming process> In the film-forming process, the film-forming raw material prepared in the dissolving process is formed into a film, and if necessary, is dried to prepare a water-soluble film with a specific moisture content.As the film-forming method, for example, a melt extrusion method or a casting method can be adopted, and the casting method is preferred in terms of the accuracy of the film thickness.When performing the casting method, for example, the film-forming raw material is extruded from a slit such as a T-slit die, cast onto a casting surface such as a plastic substrate surface of a polyethylene terephthalate film, such as the metal surface of an endless belt or a drum roll, dried, and if necessary, further heat-treated, thereby producing a water-soluble film.
[0084] The water-soluble film peeled from the casting surface, such as the surface of a plastic substrate, during the film-forming process is transported and wound up around a core tube to obtain a film roll. The obtained film roll can be supplied as a product as is, but preferably, the water-soluble film can also be supplied as a film roll obtained by slitting the water-soluble film to a film width of a desired size.
[0085] The surface of the obtained water-soluble film may be plain, but from the viewpoints of blocking resistance, slipperiness during processing, reduced adhesion between products, and appearance, it is also preferable to provide one or both sides of the film with a textured finish such as an embossed pattern, a fine textured pattern, or a specially engraved design.
[0086] The thickness of the water-soluble film is appropriately selected depending on the application, etc., but is preferably 10 to 120 μm, particularly preferably 15 to 110 μm, and even more preferably 20 to 100 μm. If the thickness is too thin, the mechanical strength of the film tends to decrease, while if the thickness is too thick, the dissolution rate in water tends to be slow and the film-forming efficiency also tends to decrease.
[0087] The width of the water-soluble film is appropriately selected depending on the application, etc., but is preferably 300 to 5000 mm, particularly preferably 500 to 4000 mm, and further preferably 600 to 3000 mm. If the width is too narrow, productivity tends to decrease, while if the width is too wide, it tends to become difficult to control slack and film thickness.
[0088] The length of the water-soluble film is appropriately selected depending on the application, etc., but is preferably 100 to 20,000 m, particularly preferably 800 to 15,000 m, and even more preferably 1,000 to 10,000 m. If the length is too short, the productivity tends to decrease because of the time and effort required to switch films, while if the length is too long, poor appearance tends to occur due to tight winding.
[0089] The water content of the water-soluble film is preferably 3 to 15% by mass, particularly preferably 5 to 9% by mass, and even more preferably 6 to 8% by mass, from the viewpoints of mechanical strength and heat sealability. If the water content is too low, the film becomes too hard, which tends to reduce the formability when made into a package and the impact resistance of the package. If the water content is too high, blocking tends to occur. The water content can be adjusted by appropriately setting the drying conditions and humidity control conditions. The water content is measured in accordance with JIS K 6726 3.4, and the value of the volatile content obtained is taken as the water content.
[0090] When the water-soluble film is used to package a neutral to weakly alkaline liquid detergent, the decrease in solubility of the film over time is inhibited, and when the water-soluble film is allowed to stand in contact with a mixed solution of 6.2% by mass of propylene glycol, 10.9% by mass of glycerin, 7.6% by mass of ethanolamine, and 12.5% by mass of water, pH 7.5, for 3 weeks, the increase in the dissolution time of the film is preferably less than 70%, particularly preferably 65% or less, even more preferably 60% or less, and especially preferably 50% or less.
[0091] The water-soluble film may be used as a single layer, or may be used as a multilayer structure in which other films or resin layers are laminated.
[0092] The water-soluble film is particularly useful for packaging chemicals such as pesticides and detergents (unit packaging) and for edible food packaging. The food to be packaged with the film may be in the form of granules, tablets, powder, etc., and is preferably dried food such as ingredients and toppings for instant foods.
[0093] <<Medicine Package>> A pharmaceutical package according to one embodiment of the present invention (hereinafter sometimes referred to as "the package") is formed by coating a pharmaceutical with a package made of the obtained water-soluble film. In this package, the pharmaceutical is packaged in a package made of a water-soluble film. When the pharmaceutical is placed in water, the surface package (water-soluble film) dissolves, exposing the pharmaceutical, which then dissolves or disperses in the water, thereby exerting its effects. Therefore, the package is suitable as a pharmaceutical package that contains a relatively small amount of pharmaceutical, such as a single dose.
[0094] Examples of the above-mentioned chemicals include agricultural chemicals such as insecticides, fungicides, and herbicides, fertilizers, detergents, etc., and detergents such as laundry detergents and dishwashing detergents are particularly preferred. Such chemicals may be liquid or solid, and if solid, may be in the form of granules, tablets, powder, etc. The chemicals are preferably those that are dissolved or dispersed in water, and are particularly preferably those that contain liquid detergents. The pH of such chemicals may be alkaline, neutral, or acidic.
[0095] The liquid detergent preferably has a pH value of 6 to 12 when dissolved or dispersed in water to a concentration of 1% by mass, particularly preferably 6 to 10, even more preferably 6.5 to 9, and especially preferably 7 to 8. The water content of the liquid detergent is preferably 15% by mass or less, particularly preferably 0.1 to 10% by mass, and even more preferably 0.1 to 7% by mass. When the water content of the liquid detergent is within the above range, the water-soluble film tends to be free from gelation or insolubilization, and the water solubility tends to be excellent. The pH value is measured in accordance with JIS K 3362 8.3. The water content is measured in accordance with JIS K 3362 7.21.3.
[0096] <<Manufacturing of Drug Package>> A known method can be used to package a drug such as a liquid detergent using a water-soluble film to form a drug package. For example, the drug package can be manufactured by the steps of preparing a first water-soluble film, a second water-soluble film, and a drug, placing the first water-soluble film and the second water-soluble film opposite each other with the drug interposed therebetween and partially abutting the first water-soluble film and the second water-soluble film, and crimping the abutting portion of the first water-soluble film and the second water-soluble film.
[0097] Specifically, a film (bottom film) is fixed to the lower mold of a molding device, and the bottom film is molded into a shape that conforms to the lower mold (a shape that allows a drug to be placed inside). Meanwhile, a film (top film) is also fixed to the upper mold of the molding device. A drug, such as a liquid detergent, prepared separately is then placed (injected) into the molded bottom film, and the molds are then pressed together to bring the top film and bottom film into contact, and the contact area is then vacuum-bonded. After the pressure bonding, the vacuum is released to obtain a drug package in which the drug is encapsulated in a water-soluble film.
[0098] Examples of methods for bonding the film include heat sealing, water sealing, and glue sealing. Of these, water sealing is preferred because it allows for easy control of bonding conditions.
[0099] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the invention. In the examples, "parts" means parts by mass.
[0100] The following materials were prepared as the water-soluble film components:
[0101] (Gelatin) (1) "#200" manufactured by Nitta Gelatin Co., Ltd.: alkali-treated (2) "Gelatin 21" manufactured by Nitta Gelatin Co., Ltd.: alkali-treated (3) "FGL-250TS" manufactured by Nitta Gelatin Co., Ltd.: acid-treated
[0102] (PVA-based resin (A)) Modified PVA-based resin (a1): a carboxyl-modified PVA-based resin having a viscosity of 22 mPa·s in a 4% aqueous solution at 20°C, an average saponification degree of 94 mol%, and a modification amount of 2.0 mol% with maleic acid monomethyl ester. Unmodified PVA resin (a2): a viscosity of 43 mPa·s in a 4% aqueous solution at 20°C, an average saponification degree of 88 mol%.
[0103] (Plasticizers) Plasticizer (b1): sorbitol Plasticizer (b2): glycerin
[0104] (Other additives) Filler: Starch (average particle size 20 μm) Surfactant: Polyoxyalkylene alkyl ether phosphate ester monoethanolamine salt
[0105] Example 1: 30 parts of gelatin, 70 parts of anionic group-modified PVA-based resin (a1) as PVA-based resin (A), 20 parts of sorbitol (b1) and 20 parts of glycerin (b2) as plasticizers (B), 0.2 parts of polyoxyalkylene alkyl ether phosphate ester monoethanolamine salt as surfactant, and water were mixed and dissolved to obtain a film-forming raw material, which was an aqueous dispersion of a resin composition with a solids concentration of 25%. The obtained film-forming raw material was allowed to stand at 60°C for 24 hours to degas. The film-forming raw material after standing and degassing was cast onto a polyethylene terephthalate film and dried by passing it through a 3-m drying chamber (105°C) at a speed of 0.440 m / min to obtain a water-soluble film with a thickness of 87 μm (water content: 7% by mass).
[0106] The obtained water-soluble films were evaluated for compatibility, solubility, mechanical properties, and water-sealing properties according to the methods described below.
[0107] <Compatibility> [Evaluation method] The presence or absence of a sea-island structure in the water-soluble film was observed using a laser microscope and evaluated based on the following criteria: [Evaluation criteria] ○ (Very good): The sea-island structure was small and phase separation was almost not observed. × (Poor): The islands in the sea-island structure were large and phase separation was evident.
[0108] <Solubility> [Evaluation method] The water-soluble film obtained above was cut into a size of 35 mm x 35 mm, placed in a 1-liter beaker containing 1 liter of water, and fixed with a jig. The film was stirred with a stirrer (rotor length 30 mm, rotation speed 750 rpm) while maintaining the water temperature at 20°C. The film was deemed to be dissolved when no dispersed insoluble fine particles with a diameter of 1 mm or more were observed, and the time required for dissolution was evaluated based on the following criteria. [Evaluation criteria] ○ (Very good): Dissolved in less than 90 seconds. △ (Good): Dissolved in 90 to 300 seconds. × (Poor): Not dissolved even after 300 seconds or more.
[0109] <Mechanical Properties> [Evaluation Method] The tensile strength and tensile elongation of the water-soluble film obtained above were measured in accordance with JIS K 7127. That is, the water-soluble film was allowed to stand for 24 hours under humidity-controlled conditions of 23°C and 50% RH before measurement, and then, under these conditions, the tensile strength and tensile elongation of the water-soluble film were measured using an Autograph AG-X Plus (manufactured by Shimadzu Corporation) at a pulling rate of 200 mm / min (film width: 15 mm, chuck distance: 50 mm). These measured values were evaluated based on the following criteria. [Evaluation Criteria] ◯ (Very good): The tensile strength was 10 MPa or more and the tensile elongation was more than 300%. Δ (Good): The tensile strength was 10 MPa or more and the tensile elongation was 200 to 300%. × (Poor): The tensile strength was 0 to less than 10 MPa and / or the tensile elongation was less than 200%.
[0110] <Water sealing property> [Evaluation method] The water-soluble film obtained above was cut into a size of 100 mm × 200 mm (top film) and 100 mm × 100 mm (bottom film), and a water sealing test was performed. That is, the water-soluble film was left to stand for 24 hours under humidity conditions of 23 ° C. and 40% RH, and then, under this environment, the water-soluble film (bottom film) was fixed on a 30 cm square glass plate, and water was applied using a water-soaked PVA sponge roller ("Cygnus Roller" manufactured by Ion Co., Ltd.). Thereafter, the water-soluble film (top film) was placed on the water-coated water-soluble film (bottom film), and another rubber roller (width 250 mm, diameter 60 mm, weight 2750 g) was rolled twice from above to press the top film and bottom film together, thereby preparing a test specimen. After 2 minutes had passed, the test piece was used to measure the peel strength of the sealed portion using an Autograph AG-X Plus (manufactured by Shimadzu Corporation) at a tensile speed of 100 mm / min (film width 15 mm, chuck distance 20 mm). The state of failure of the sealed portion in the water seal test, or the average test force over a stroke of 50 to 100 mm, was evaluated based on the following criteria: [Evaluation criteria] ◯ (Very good): The average test force was 5 N / 15 mm or more, and cohesive failure occurred in the water sealed portion. △ (Good): The average test force was 5 N / 15 mm or more, and interfacial peeling occurred in the water sealed portion. × (Poor): The average test force was less than 5 N / 15 mm.
[0111] Examples 2 to 6, Comparative Example 1 Water-soluble films were obtained in the same manner as in Example 1, except for the changes shown in Table 1. The obtained water-soluble films were evaluated in the same manner as in Example 1. The results are shown in Table 1 below.
[0112]
[0113] It can be seen that the water-soluble films of Examples 1 to 6, which contain gelatin and a modified PVA-based resin, have good compatibility between the gelatin and the PVA-based resin and excellent solubility. They also have excellent mechanical properties and water-tightness, making them suitable for packaging applications. On the other hand, the water-soluble film of Comparative Example 1, which does not contain a modified PVA-based resin as the PVA-based resin, has poor compatibility with gelatin and is inferior in solubility and mechanical properties, making it unsuitable for practical use.
[0114] <Preparation of Packages> Packages were prepared using the water-soluble films of Examples 2, 4, and 5 obtained above using an Engel packaging machine according to the following procedure. Specifically, the water-soluble films were left to stand for 24 hours under humidity-controlled conditions of 23°C and 40% RH. After this, a PVA-based water-soluble film (bottom film) was fixed onto a mold (package to be molded: length 45 mm, width 42 mm, height 30 mm) at the bottom of the machine, and a PVA-based water-soluble film (top film) was also fixed onto the top of the machine. The bottom film was heated for 4 seconds using a dryer generating hot air at 70°C, and the bottom film was vacuum-molded into the mold. Then, 25 mL of a commercially available liquid laundry detergent (composition summary: 11% by mass propylene glycol, 7.5% by mass glycerin, 67% by mass surfactant, 14.2% by mass water, pH 7.5 (undiluted)) was poured into the molded water-soluble film. 0.25 g of water was applied to the entire surface of the top film (80 mm long, 140 mm wide), and the top film and bottom film were pressed together for 10 seconds, after which the vacuum was released to produce a package.
[0115] The resulting packaging was evaluated for compressive strength and film solubility over time according to the methods described below. The results are shown in Table 2.
[0116] <Compression Strength> [Evaluation Method] After 1 hour, the packages prepared by the above method were measured for compressive strength at the time of package rupture using an Autograph AG-X Plus (Shimadzu Corporation) at a test speed of 200 mm / min. A 5 kN load cell was used. [Evaluation Criteria] ○ (Very good): The compressive strength was greater than 500 N. △ (Good): The compressive strength was 200 to 500 N. × (Poor): The compressive strength was less than 200 N and the package was easily ruptured.
[0117] <Solubility over time> [Evaluation method] Following the above-described package preparation procedure, a package manufacturing machine manufactured by Engel was used to prepare packages in which liquid laundry detergents of various pH values (Detergent 1 composition summary: 6.2% by mass of propylene glycol, 10.9% by mass of glycerin, 7.6% by mass of ethanolamine, 12.5% by mass of water, pH 7.0 (undiluted)) (Detergent 2 composition summary: 11.2% by mass of propylene glycol, 13.4% by mass of glycerin, 8.4% by mass of ethanolamine, 11.8% by mass of water, pH 9.5 (undiluted)) were wrapped in a water-soluble film. The packages were placed in a thermo-hygrostat and left at 37°C and 70% RH for 3 weeks with the water-soluble film and detergent in contact. After that, the liquid detergent adhering to the film was wiped off, and the solubility of the film was tested at 20°C in the same manner as in the solubility measurement described above. [Evaluation criteria] The rate of increase in the time required for dissolution of the water-soluble film was determined as follows to evaluate solubility over time. Increase rate (%) = [{time required for film to dissolve after 3 weeks (sec)} - {time required for water-soluble film to dissolve when producing package (sec)}] / time required for water-soluble film to dissolve when producing package (sec) (Detergent 1: pH 7.0) ◯ (Very good): Increase rate was less than 70%. △ (Good): Increase rate was 70-100%. × (Poor): Increase rate was greater than 100%. (Detergent 2: pH 9.5) ◯ (Very good): Increase rate was less than 70%. △ (Good): Increase rate was 70-100%. × (Poor): Increase rate was greater than 100%.
[0118]
[0119] The water-soluble films of Examples 2, 4, and 5 containing gelatin and modified PVA-based resin have sufficient compressive strength when used as packaging materials, and are therefore suitable for packaging liquid medicines and foods. Furthermore, the solubility of the films does not decrease over time even when packaging liquid detergents, and in particular, the solubility of the films does not decrease over time even when packaging neutral to weakly alkaline detergents, making them suitable for packaging liquid laundry detergents.
[0120] Although the above examples show specific embodiments of the present invention, the examples are merely illustrative and should not be construed as limiting. Various modifications that are obvious to those skilled in the art are intended to fall within the scope of the present invention.
[0121] The water-soluble film of the present invention can be used for packaging (unit packaging) of chemicals such as pesticides and detergents, transfer films, sanitary products such as napkins and disposable diapers, waste disposal products such as ostomy bags, medical products such as blood-absorbing sheets, and temporary substrates such as seedling raising sheets, seed tapes, and embroidery base fabrics. Furthermore, the film of the present invention, which is a blend film of naturally derived raw materials and a PVA-based resin also used in foods and pharmaceuticals, is also useful for edible applications (food packaging) and cosmetic packaging.
Claims
1. A water-soluble film comprising gelatin and a polyvinyl alcohol-based resin (A), the polyvinyl alcohol-based resin (A) comprising a modified polyvinyl alcohol-based resin.
2. The water-soluble film according to claim 1, wherein the modified polyvinyl alcohol resin contains at least one modified polyvinyl alcohol resin selected from the group consisting of anionic group-modified polyvinyl alcohol, pyrrolidone ring group-modified polyvinyl alcohol, and amino group-modified polyvinyl alcohol.
3. The water-soluble film according to claim 1 or 2, further comprising a plasticizer.
4. A water-soluble film according to any one of claims 1 to 3, having a moisture content of 3 to 15% by mass.
5. The water-soluble film according to any one of claims 1 to 4, which is used for packaging medicines.
6. The water-soluble film according to any one of claims 1 to 5, wherein when the water-soluble film is allowed to stand in contact with a mixed solution of 11.2% by mass of propylene glycol, 13.4% by mass of glycerin, 8.4% by mass of ethanolamine, and 11.8% by mass of water, pH 9.5, the increase in the dissolution time of the film is less than 70% when the water-soluble film is allowed to stand for three weeks.
7. The water-soluble film according to any one of claims 1 to 6, wherein when the water-soluble film is allowed to stand in contact with a mixed solution of 6.2% by mass of propylene glycol, 10.9% by mass of glycerin, 7.6% by mass of ethanolamine, and 12.5% by mass of water, pH 7.0, the increase in the dissolution time of the film is less than 70% when the film is allowed to stand in contact with the mixed solution for 3 weeks.
8. A pharmaceutical package comprising a package made of the water-soluble film according to any one of claims 1 to 7 and a pharmaceutical packaged therein.
9. The pharmaceutical package of claim 8, wherein the pharmaceutical is a liquid detergent.
10. The pharmaceutical package according to claim 9, wherein the liquid detergent has a pH value of 6 to 9 when dissolved or dispersed in water.
11. A method for producing a water-soluble film according to any one of claims 1 to 7, comprising the steps of: preparing a film-forming raw material containing gelatin and a modified polyvinyl alcohol resin; casting the film-forming raw material onto a casting surface; and drying the cast film-forming raw material.
12. A method for producing a pharmaceutical package as described in any one of claims 8 to 10, comprising the steps of: preparing a first water-soluble film, a second water-soluble film, and a pharmaceutical package; placing the first water-soluble film and the second water-soluble film opposite each other with the pharmaceutical package interposed between them; and partially abutting the first water-soluble film and the second water-soluble film; and crimping the abutting portion between the first water-soluble film and the second water-soluble film.
Citation Information
Patent Citations
Edible film and its production
JP1994105660A
Soluble packing material
JP1994183456A
Edible film
JP2002095426A
Edible film
JP2008079525A
High-molecular material composition
JP1987121765A
Cited By
Water-soluble film, method for producing same, package, medicine package, and method for producing same
WO2025205906A1