Three-dimensional net-like structure and manufacturing method for same

The three-dimensional network structure with a high polybutylene adipate terephthalate content and differential absorbance allows for visual differentiation between sides, addressing the challenge of distinguishing between front and back sides in cushioning materials without colored markers, ensuring consistent performance.

WO2024204151A1PCT designated stage expired Publication Date: 2024-10-03TOYOBO MC CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011867
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-26
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Cushioning materials for bedding and pillows lack a method to visually distinguish between the front and back sides without using colored materials, leading to potential changes in feel and difficulty in correct orientation.

Method used

A three-dimensional network structure with a random loop bonded structure composed of continuous filaments, where the thermoplastic resin composition contains 70% or more polybutylene adipate terephthalate, and the difference in absorbance at 500 nm between the two surfaces is 0.020 or more, allowing for visual differentiation.

Benefits of technology

Enables easy visual distinction between the front and back sides of the cushioning material without using colored materials, maintaining consistent feel and properties on both sides.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011867_03102024_PF_FP_ABST
    Figure JP2024011867_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a three-dimensional net-like structure the front and rear sides of which can be visually discriminated without using a colored material. Provided is a three-dimensional network structure having a three-dimensional random loop junction structure composed of continuous filaments, the three-dimensional network structure being characterized in that: the continuous filaments contain 70 mass% or more of polybutylene adipate terephthalate; and, regarding two surfaces facing each other in the thickness direction of the three-dimensional network structure, the absolute value of the difference between absorbance at a wavelength of 500 nm on one of the two surfaces and absorbance at a wavelength of 500 nm on the other surface is 0.020 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Three-dimensional network structure and manufacturing method thereof

[0001] The present invention relates to a three-dimensional network structure and a method for producing the same.

[0002] Up until now, three-dimensional network structures have been widely used as cushioning materials for bedding such as furniture and beds, and for seats in vehicles such as trains, automobiles, motorcycles, etc., because of their excellent breathability and recyclability. Furthermore, with the recent acceleration of efforts to address environmental issues, research has been progressing on three-dimensional network structures using biodegradable polymers that decompose in a shorter time than conventional polymers, and various technologies for biodegradable three-dimensional network structures have been disclosed so far.

[0003] When cushioning materials are used for bedding, pillows, etc., it is common to remove the cover from the cushioning material and wash it, or to wash the cover and cushioning material separately, from the standpoint of hygiene and cleanliness.

[0004] For example, Patent Document 1 discloses a cushion filling material in which a soft urethane foam having open cells and / or interconnected spaces is laminated on one or both sides of a three-dimensional mesh structure, making it possible to easily wash the cushion material with water from a hygienic standpoint.

[0005] JP 2017-226230 A JP 2019-181247 A

[0006] Cushioning materials used in bedding and pillows have different properties on the front side, which comes into contact with the human body, and the back side, which is the reverse side. However, when cushioning material is removed from a cover and then put back into the cover, it is difficult to visually distinguish between the front and back of the cushioning material, which can be a time-consuming task. In addition, if cushioning material is put back into the cover with the wrong front and back, the feel of the material will unintentionally change from the feel it had just felt when used.

[0007] Therefore, in order to obtain the same feel as before removing the cover, it is desirable to be able to easily visually determine the front and back of the cushioning material. However, because the cushioning material in Patent Document 1 has a mesh structure that is uniform in the thickness direction, it is difficult to determine the previously used side once it is removed from the cover. On the other hand, Patent Document 2 discloses a mattress core material in which marking material is intermittently inserted along the mattress longitudinal direction, making it possible to visually determine the front and back. However, Patent Document 2 requires the use of a separate colored material for marking, leaving room for improvement.

[0008] An object of the present invention is to provide a three-dimensional netted structure whose front and back can be visually distinguished without using a colored material.

[0009] As a result of intensive research to solve the above-mentioned problems, the inventors have found that it is possible to distinguish between the front and back of a three-dimensional network structure by increasing the difference between the absorbance at a wavelength of 500 nm on one side of the three-dimensional network structure and the absorbance at a wavelength of 500 nm on the other side.

[0010] That is, the present invention includes the following inventions. [1] A three-dimensional network structure having a three-dimensional random loop bonded structure composed of continuous filaments, wherein the thermoplastic resin composition constituting the continuous filaments contains 70% by mass or more of polybutylene adipate terephthalate, and the absolute value of the difference between the absorbance at a wavelength of 500 nm on one surface and the absorbance at a wavelength of 500 nm on the other surface facing each other in the thickness direction of the three-dimensional network structure is 0.020 or more. [2] The three-dimensional network structure according to [1] above, wherein the polybutylene adipate terephthalate contains adipic acid units and terephthalic acid units, and the molar ratio of the terephthalic acid units to the adipic acid units is 0.8 or more and 3.0 or less. [3] The three-dimensional network structure according to [1] or [2] above, which is used as a cushioning material. [4] A method for producing the three-dimensional network structure according to [1] or [2] above, comprising: an extrusion step of extruding the molten thermoplastic resin composition from a nozzle; a molding step of obtaining a molded body molded into a three-dimensional network structure using the continuous filaments discharged from the nozzle; and a heat treatment step of heat-treating the molded body, wherein the molding step comprises a step of immersing the continuous filaments in water in a water tank and a step of partially cooling the continuous filaments with a water discharge device, and the cooling water discharged from the water discharge device has a temperature 5°C or more lower than that of the water in the water tank.

[0011] In the present invention, the front and back of the three-dimensional network structure can be distinguished by increasing the difference between the absorbance at a wavelength of 500 nm on one side of the three-dimensional network structure and the absorbance at a wavelength of 500 nm on the other side.

[0012] 1 is a schematic diagram of a network structure manufacturing apparatus according to an embodiment of the present invention, a network structure manufacturing apparatus according to another embodiment of the present invention, and a schematic diagram of a network structure manufacturing apparatus according to the embodiment of the present invention, as viewed from above.

[0013] The three-dimensional network structure of the present invention has a three-dimensional random loop bonded structure composed of continuous filaments.

[0014] On two opposing surfaces in the thickness direction of the three-dimensional network structure, the absolute value of the difference between the absorbance at a wavelength of 500 nm on one surface and the absorbance at a wavelength of 500 nm on the other surface (hereinafter referred to as the absorbance difference between both surfaces) is 0.020 or more. When the absorbance difference between both surfaces is 0.020 or more, the colors of one surface and the other surface are significantly different. As a result, the front and back of the three-dimensional network structure can be easily distinguished visually. Even in a three-dimensional network structure with different fiber diameters in the thickness direction, visual distinction is made easier when the absorbance difference between both surfaces is 0.020 or more. The absorbance difference between both surfaces is preferably 0.035 or more, more preferably 0.060 or more. The upper limit of the absorbance difference between both surfaces is not particularly limited, but due to technical difficulties, it is, for example, 0.200 or less. The absorbance difference between both surfaces can be measured using a spectrophotometer, spectrophotometer, or the like, and can be measured, for example, by the measurement method described in the Examples below. Each component will be described in detail below.

[0015] <Thermoplastic Resin Composition> The thermoplastic resin composition constituting the continuous filaments contains 70% by mass or more of polybutylene adipate terephthalate resin. By selecting polybutylene adipate terephthalate resin from biodegradable resins and using a thermoplastic resin composition containing 70% by mass or more of polybutylene adipate terephthalate resin relative to 100% by mass of the thermoplastic resin composition, a biodegradable three-dimensional network structure with excellent cushioning properties can be obtained. The content of the polybutylene adipate terephthalate resin relative to the thermoplastic resin composition is preferably 75% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more. Furthermore, the thermoplastic resin composition constituting the continuous filaments may be 100% by mass of polybutylene adipate terephthalate resin.

[0016] Polybutylene adipate terephthalate resin is a biodegradable resin and a copolymer of adipic acid, terephthalic acid, and butanediol. Because of its biodegradability, polybutylene adipate terephthalate resin is expected to be a solution to waste disposal and microplastic problems. Adipic acid, terephthalic acid, and butanediol do not need to be copolymerized simultaneously; they may be copolymerized in multiple stages. Furthermore, polybutylene adipate terephthalate resin is preferably a thermoplastic resin.

[0017] In the polybutylene adipate terephthalate resin, the molar ratio of terephthalic acid units to adipic acid units is preferably 0.8 or more and 3.0 or less. The lower limit of the molar ratio is more preferably 1.0 or more, even more preferably 1.1 or more, and particularly preferably 1.2 or more. On the other hand, the upper limit of the molar ratio is more preferably 2.5 or less, even more preferably 2.0 or less. When the molar ratio is 0.8 or more, the compression recovery after heat compression at the usage temperature of the three-dimensional network structure is easily improved. On the other hand, when the molar ratio is 3.0 or less, flexibility is improved. Therefore, it is suitable for cushioning materials, etc.

[0018] The melting point of the polybutylene adipate terephthalate resin is preferably 120°C or higher and 180°C or lower. The lower limit of the melting point is more preferably 125°C or higher, even more preferably 130°C or higher, still more preferably 140°C or higher, and particularly preferably 145°C or higher. On the other hand, the upper limit of the melting point is more preferably 170°C or lower, even more preferably 160°C or lower. A melting point of 120°C or higher can easily improve the compression recovery after heat compression at the usage environment temperature of the three-dimensional network structure. On the other hand, a melting point of 180°C or lower improves flexibility, making it suitable for use as a cushioning material, etc.

[0019] The melt flow rate (MFR) of the polybutylene adipate terephthalate resin is preferably 3 g / 10 min to 60 g / 10 min. An MFR of 3 g / 10 min or higher can increase the melt viscosity and the fiber diameter of the continuous filaments. The lower limit of the MFR is more preferably 5 g / 10 min or higher, even more preferably 12 g / 10 min or higher, even more preferably 15 g / 10 min or higher, and particularly preferably 18 g / 10 min or higher. On the other hand, an MFR of 60 g / 10 min or lower facilitates improved compression recovery after heat compression. The upper limit of the MFR is more preferably 50 g / 10 min or lower, even more preferably 40 g / 10 min or lower, and particularly preferably 30 g / 10 min or lower. The MFR of the thermoplastic resin composition constituting the continuous filaments is also preferably within the above range. The MFR of the resin can be measured by the method described in the Examples below.

[0020] When a commercially available resin is used as the polybutylene adipate terephthalate resin, if the resin has a low melt flow rate (MFR), the MFR of the resin can be increased by adding water to the resin to hydrolyze the resin during melt extrusion. On the other hand, if the resin has a high MFR, the MFR of the resin can be decreased by drying the resin before melt extrusion.

[0021] The weight-average molecular weight (g / mol) of the polybutylene adipate terephthalate resin is preferably 35,000 or more. This can improve compression recovery after heat compression. The weight-average molecular weight is more preferably 37,000 or more, and even more preferably 40,000 or more. On the other hand, the weight-average molecular weight is preferably 150,000 or less, which can improve flexibility. It is more preferably 120,000 or less. Furthermore, the weight-average molecular weight (g / mol) of the thermoplastic resin constituting the continuous filaments is also preferably within the same range. The weight-average molecular weight can be determined by gel permeation chromatography (GPC) or the like.

[0022] The thermoplastic resin composition constituting the continuous filaments may contain a biodegradable resin other than polybutylene adipate terephthalate resin. Preferred examples of such other biodegradable resins include polylactic acid, polylactic acid / polycaprolactone copolymer, polylactic acid / polyether copolymer, polyethylene terephthalate succinate, polybutylene succinate, polybutylene succinate adipate, polyglycolic acid, polycaprolactone, polyvinyl alcohol, and cellulose acetate. These may be used alone or in combination of two or more. For details, please refer to the positive list of GreenPla (biodegradable plastic) classification number A-1 of the Japan BioPlastics Association. The thermoplastic resin composition constituting the continuous filaments may contain a resin other than biodegradable resin. Examples of such resins include thermoplastic resins such as polyolefin, polyurethane, and polyester.

[0023] The thermoplastic resin composition constituting the continuous filaments may contain deodorants, antibacterial agents, antifungal agents, antimite agents, deodorizers, antifungal agents, aromatic agents, flame retardants, moisture absorbing and releasing agents, antioxidants, lubricants, etc. These may be used alone or in combination of two or more.

[0024] The thermoplastic resin composition constituting the continuous filaments may contain, in addition to the polybutylene adipate terephthalate resin, a resin containing a copolymerization component other than adipic acid, terephthalic acid, and butanediol as a unit. Examples of the copolymerization component include dicarboxylic acids other than terephthalic acid and adipic acid, diols other than butanediol, polyalkylene glycols, and modifiers for the purposes of chain extension, terminal blocking, etc. These may be used alone or in combination of two or more.

[0025] Other dicarboxylic acids include oxalic acid, malonic acid, succinic acid, glutaric acid, pimelic acid, suberic acid, etc. These may be used alone or in combination of two or more.

[0026] Examples of other diols include methanediol, ethanediol, propanediol, pentanediol, and hexanediol. Examples of polyalkylene glycols include polymethylene glycol, polyethylene glycol, polypropylene glycol, and polybutylene glycol (polytetramethylene glycol). These may be used alone or in combination of two or more.

[0027] Examples of the modifier include polyisocyanate compounds and glycol compounds. Examples of the polyisocyanate compound include diisocyanate compounds. Examples of the diisocyanate compound include hexamethylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, xylylene diisocyanate, 1,5-naphthylene diisocyanate, p-phenylene diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, tetramethylxylene diisocyanate, carbodiimide-modified MDI, and polymethylene phenyl polyisocyanate. These may be used alone or in combination of two or more.

[0028] Petroleum-derived monomers may be used as monomers for synthesizing the thermoplastic resin composition constituting the continuous filaments. However, it is preferable to use biomass-derived monomers from the viewpoint of reducing the environmental load. As the biomass-derived monomers, for example, monomers listed in the positive list of classification number A (biomass plastics) of the Japan Bioplastics Association can be used.

[0029] The total content of adipic acid units and terephthalic acid units relative to 100 mol% of dicarboxylic acid units contained in the thermoplastic resin composition constituting the continuous filaments is preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 90 mol% or more, still more preferably 95 mol% or more, and particularly preferably 99 mol% or more. Furthermore, the content of butanediol units relative to 100 mol% of diol units contained in the thermoplastic resin composition constituting the continuous filaments is preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 90 mol% or more, still more preferably 95 mol% or more, and particularly preferably 99 mol% or more.

[0030] <Continuous Filaments> The three-dimensional network structure of the present invention is composed of continuous filaments made of a thermoplastic resin composition and has a three-dimensional random loop bonded structure. The continuous filaments are linear filaments having a continuous portion of at least 5 mm or more. The three-dimensional network structure is easily formed by having portions where the intersections of the continuous filaments are bonded. Therefore, it is preferable that the three-dimensional network structure has bonded portions where the intersections of the continuous filaments are bonded to each other.

[0031] The continuous filament may be a composite filament of a sheath-core type, a side-by-side type, an eccentric sheath-core type, or the like. The composite filament may be a composite filament combining a polybutylene adipate terephthalate resin with another thermoplastic resin, or a composite filament combining polybutylene adipate terephthalate resins with different composition ratios. The cross-sectional shape of the continuous filament may be either a hollow or solid cross-section, with a hollow cross-section being preferred from the viewpoint of weight reduction. Fibers with different cross-sectional shapes in the thickness direction or width direction may also be combined. Furthermore, the cross-sectional shape of the continuous filament is preferably a modified cross-section. This makes it easier to impart suitable hardness and cushioning properties to the three-dimensional network structure. The lower limit of the hollow ratio of the continuous filament is preferably 1% or more, more preferably 2% or more, and particularly preferably 5% or more. On the other hand, the upper limit of the hollow ratio of the continuous filament is preferably 30% or less, more preferably 25% or less, and particularly preferably 20% or less. The hollow ratio of the continuous filament can be measured by the method described in the Examples below.

[0032] The average fiber diameter of the continuous filaments is preferably 0.2 mm to 2.0 mm. An average fiber diameter of 0.2 mm or more improves hardness. Therefore, the average fiber diameter is more preferably 0.3 mm or more, and even more preferably 0.4 mm or more. On the other hand, an average fiber diameter of 2.0 mm or less improves the density of the network structure, thereby improving cushioning properties and making it easier to make the network structure feel soft. Therefore, the average fiber diameter is more preferably 1.7 mm or less, even more preferably 1.5 mm or less, and particularly preferably 1.2 mm or less. The average fiber diameter of the continuous filaments can be measured by the method described in the Examples below.

[0033] The continuous filaments preferably have a melting enthalpy of 16 J / g or more. Having a melting enthalpy of 16 J / g or more can improve the compression durability of the three-dimensional network structure and its compression recovery after heat compression. The melting enthalpy is more preferably 17 J / g or more, even more preferably 18 J / g or more, even more preferably 19 J / g or more, even more preferably 20 J / g or more, and particularly preferably 21 J / g or more. On the other hand, the melting enthalpy is preferably 30 J / g or less. This improves the flexibility of the three-dimensional network structure and reduces the generation of noise during compression and recovery. The melting enthalpy is more preferably 28 J / g or less, even more preferably 26 J / g or less.

[0034] The enthalpy (J / g) of the endothermic peak of the continuous filament can be determined from the integral of the endothermic peak (melting peak) from a DSC curve measured with a sample mass of 2.0 mg±0.1 mg using a differential scanning calorimeter under a nitrogen atmosphere at a heating rate of 20° C. / min. The integral can be determined by setting the point at which the curve relating to the endothermic peak (melting peak) starts to deviate from the baseline on the low temperature side as the starting point and the point at which it starts to contact the baseline on the high temperature side as the end point, drawing a straight line connecting the starting point and the end point, and integrating the area enclosed by the straight line and the curve.

[0035] <Three-dimensional network structure> The three-dimensional network structure may have a multilayer structure. Examples of the multilayer structure include a structure in which the surface layer and the back layer are made of continuous filaments with different finenesses, a structure in which the surface layer and the back layer are made of structures with different apparent densities, or a structure in which long-fiber nonwoven fabrics, short-fiber nonwoven fabrics, etc. are laminated. Examples of the multilayer structure method include a method of melt-bonding by heating, a method of bonding with an adhesive, a method of restraining with sewing or a band, etc.

[0036] The shape of the three-dimensional network structure is not particularly limited. Examples include a plate, a polygon such as a triangular prism or a quadrangular prism, a cylinder, a sphere, a combination of these, etc. When molding the three-dimensional network structure, a regulating plate may be used during melt extrusion of the resin, or the structure may be molded by cutting, heat pressing, etc.

[0037] The apparent density of the three-dimensional network structure is preferably 0.005 g / cm 3 ~0.30 g / cm 3 The apparent density is 0.005 g / cm 3 By setting the apparent density at or above 0.01 g / cm3, the hardness of the three-dimensional network structure is improved. As a result, when the three-dimensional network structure is used in a cushion or the like, the feeling of hitting the bottom can be reduced. Therefore, the lower limit of the apparent density is more preferably 0.01 g / cm3. 3 More preferably, 0.02 g / cm 3 More preferably, 0.03 g / cm 3 On the other hand, the apparent density is 0.30 g / cm or more. 3 When the apparent density is 0.20 g / cm or less, the flexibility is improved and the material can be suitably used as a cushioning material, etc. Therefore, the upper limit of the apparent density is more preferably 0.20 g / cm 3 More preferably, 0.15 g / cm or less 3 The apparent density of the three-dimensional network structure can be measured by the method described in the examples below.

[0038] The thickness of the three-dimensional network structure is preferably 10 mm to 120 mm. A thickness of 10 mm or more makes it easier to use the three-dimensional network structure as a cushioning material, etc. Therefore, the lower limit of the thickness is more preferably 15 mm or more, even more preferably 20 mm or more, and particularly preferably 22 mm or more. On the other hand, taking into account the size of the manufacturing apparatus, the upper limit of the thickness is more preferably 100 mm or less, even more preferably 80 mm or less, and particularly preferably 50 mm or less. The thickness of the three-dimensional network structure can be measured by the method described in the examples below.

[0039] The three-dimensional network structure preferably has a 40°C compression set of 25% or less. This improves compression recovery after heat compression. The upper limit of the 40°C compression set is more preferably 22% or less, even more preferably 20% or less, and particularly preferably 15% or less. The 40°C compression set may be 1% or more, or may be 5% or more. The 40°C compression set can be measured by the method described in the Examples below.

[0040] The three-dimensional network structure preferably has a 70°C compression set of 30% or less. This improves compression recovery after heat compression. The upper limit of the 70°C compression set is more preferably 25% or less, and even more preferably 23% or less. The 70°C compression set may be 1% or more, or may be 5% or more. The 70°C compression set can be measured by the method described in the Examples below.

[0041] The three-dimensional network structure has a hardness at compression when compressed 25% in the thickness direction (when compressed to 75% thickness) (hereinafter referred to as "hardness at 25% compression") of preferably 5.0 N / φ200 mm or more and 100 N / φ200 mm or less. Having a hardness at 25% compression of 5.0 N / φ200 mm or more can reduce the feeling of bottoming out when the three-dimensional network structure is used as a cushioning material, etc. Therefore, the lower limit of the hardness at 25% compression is more preferably 5.4 N / φ200 mm or more, even more preferably 6.0 N / φ200 mm or more, and particularly preferably 7.0 N / φ200 mm or more. On the other hand, having a hardness at 25% compression of 100 N / φ200 mm or less can improve cushioning properties. Therefore, the upper limit of the hardness at 25% compression is more preferably 80 N / φ200 mm or less, even more preferably 60 N / φ200 mm or less, and particularly preferably 30 N / φ200 mm or less. The hardness at 25% compression can be measured by the method described in the examples below.

[0042] The melting point of the three-dimensional network structure is preferably 120°C or higher and 180°C or lower. The lower limit of the melting point is more preferably 125°C or higher, even more preferably 130°C or higher, still more preferably 140°C or higher, and particularly preferably 145°C or higher. On the other hand, the upper limit of the melting point is more preferably 170°C or lower, and even more preferably 160°C or lower. A melting point of 120°C or higher can easily improve the compression recovery of the three-dimensional network structure after heat compression at the usage environment temperature. On the other hand, a melting point of 180°C or lower improves flexibility, making it suitable for use as a cushioning material, etc.

[0043] It is preferable that the three-dimensional network structure does not contain a bonding promoter. This makes it easier to prevent excessive hardening due to excessive bonding within the three-dimensional network structure caused by the bonding promoter. It also makes it easier to prevent a decrease in the density of the three-dimensional network structure due to an excessive increase in the bonding area per contact point. Examples of the bonding promoter include polycaprolactone, polybutylene succinate, polybutylene sebacate terephthalate, and polybutylene azelate terephthalate.

[0044] The three-dimensional network structure of the present invention is suitable for use in cushions. The cushion may be any cushion that has elasticity to support an object or that reduces impact. Examples of cushions include cushions used in office chairs, furniture, sofas, beds, and other bedding; vehicle seats such as those for trains, automobiles, motorcycles, child seats, and strollers; and cushions used in impact-absorbing mats such as floor mats and collision and pinch prevention members.

[0045] <Method for Manufacturing a Three-Dimensional Network Structure> The method for manufacturing a three-dimensional network structure preferably includes an extrusion step of extruding the molten thermoplastic resin composition from a nozzle, a molding step of obtaining a molded body having a three-dimensional network structure using the continuous filaments extruded from the nozzle, and a heat treatment step of heat-treating the molded body. The three-dimensional network structure prior to the heat treatment step is referred to as a molded body to avoid confusion with the finished three-dimensional network structure (the three-dimensional network structure after the heat treatment step). The extrusion and molding steps are not particularly limited as long as they are known manufacturing methods, but specific manufacturing methods include, for example, the following. First, a thermoplastic resin composition containing a polybutylene adipate terephthalate resin is dispensed into the nozzle orifices from a multi-row nozzle having multiple orifices, and extruded downward from the nozzle at a spinning temperature of at least (the melting point + 20°C) but less than (the melting point + 180°C) of the resin. Next, the continuous filaments are brought into contact with each other in the molten state and fused to form a three-dimensional network structure, which is then sandwiched in a take-up conveyor net and cooled with water in a water tank. At this time, by cooling one side of the three-dimensional network structure with water (hereinafter referred to as cooling water) that is at a temperature lower than that of the water in the water tank, the difference in absorbance between the two sides can be increased.

[0046] The solidified molded body is then drawn out and drained or dried to obtain a molded body with one or both sides smoothed. For details of these spinning and cooling processes, see, for example, the description in JP-A-7-68061. When smoothing only one side, continuous filaments are extruded onto an inclined take-up net, and the continuous filaments are brought into contact with each other in a molten state and fused together. During this process, a three-dimensional network structure is formed, and only the take-up net surface is cooled while relaxing its shape. The obtained molded body is then subjected to a heat treatment. The drying treatment of the molded body may also be used as the heat treatment.

[0047] Polybutylene adipate terephthalate resin may undergo molding shrinkage before being cooled and solidified. Therefore, a three-dimensional network structure with a width and thickness that take molding shrinkage into consideration may be formed. For example, molding shrinkage can be reduced by lowering the melt-solidification temperature. The temperature of the water in the water tank is preferably 80°C or less, more preferably 70°C or less. The lower limit of the water temperature in the water tank is not particularly limited, and is, for example, 30°C or more. The cooling time with water is preferably 30 seconds or more. The cooling and solidification is preferably carried out in a water tank.

[0048] As described above, a method for increasing the difference in absorbance between the two surfaces can be achieved by cooling one surface of the three-dimensional network structure with cooling water at a temperature lower than that of the water in the water tank. For example, cooling water can be discharged from the outside of one of the conveyor nets or from above the conveyor net. In the method for discharging cooling water from above the conveyor net, the three-dimensional network structure does not exist on the extension of the direction in which the cooling water is discharged. Details of these methods will be described later using Figures 1 and 2.

[0049] To increase the absorbance difference between the two surfaces, the temperature of the cooling water is preferably at least 5°C lower than that of the water in the water tank, more preferably at least 10°C lower, even more preferably at least 20°C lower, and particularly preferably at least 30°C lower. A sufficient absorbance difference can be achieved when the temperature of the cooling water is at least 5°C lower than that of the water in the water tank. The three-dimensional network structure obtained by the above method has a large absorbance difference between the two surfaces, making it easy to visually distinguish between the front and back of the three-dimensional network structure. When the above manufacturing method is used, the difference in average fiber diameter between the two surfaces is small, and the value obtained by dividing the larger average fiber diameter between the two surfaces by the smaller average fiber diameter is preferably 1.0 to 1.6, more preferably 1.0 to 1.2, and even more preferably greater than 1.0 and not greater than 1.05. Furthermore, when the above-described manufacturing method is used, the difference in hardness (hardness at 25% compression, described below) between both surfaces is also small, and the value obtained by dividing the larger of the hardness values ​​between the two surfaces by the smaller of the two hardness values ​​is preferably 1.0 to 1.6, more preferably 1.0 to 1.2, and even more preferably greater than 1.0 and not greater than 1.05. Therefore, when a three-dimensional network structure is manufactured using a nozzle that is uniform in the thickness direction, a three-dimensional network structure having similar cushioning properties on both surfaces can be obtained.

[0050] Furthermore, by producing a three-dimensional network structure using the above-described production method, it is possible to produce a three-dimensional network structure that is easy to distinguish visually without using additives such as colorants. By not using additives such as colorants, the three-dimensional network structure can be recycled, and used three-dimensional network structures can be reused as raw materials for three-dimensional network structures, etc.

[0051] Water may be added to the thermoplastic resin composition before it is discharged from the nozzle. Adding water to the thermoplastic resin composition can promote hydrolysis of the thermoplastic resin during the production process of the three-dimensional network structure, thereby improving the flexibility of the resin. The amount of water added is preferably 2.0% by mass or less based on the thermoplastic resin composition. This can prevent excessive decomposition of the thermoplastic resin during the production process of the three-dimensional network structure. As a result, compression recovery after heat compression is easily improved. The method for adding water to the thermoplastic resin composition is not particularly limited. For example, before the resin is discharged from the nozzle, the thermoplastic resin composition is vacuum-dried at 100°C for 12 hours or more to completely dry it. Next, a predetermined amount of pure water can be added to 100% by mass of the completely dried thermoplastic resin composition.

[0052] The melt flow rate (MFR) of the polybutylene adipate terephthalate resin before melt extrusion is preferably at least 0.5 and less than 20.0 lower than the MFR of the continuous filaments that constitute the desired three-dimensional network structure. Since thermal degradation and shear degradation of the resin are induced during melt extrusion, controlling the MFR before melt extrusion as described above makes it easier to obtain continuous filaments having the desired MFR.

[0053] The heat treatment may be carried out using a commercially available hot air drying oven or in a warm water bath. The heat treatment is preferably carried out at a temperature at least 5°C higher than the temperature of the water in the water tank. The heat treatment temperature is preferably 50°C or higher. This allows the enthalpy of fusion to be increased. The heat treatment temperature is more preferably 60°C or higher, and even more preferably 70°C or higher. The heat treatment may be carried out in multiple steps at different temperatures.

[0054] When carrying out the heat treatment, the melting point of the thermoplastic resin composition constituting the continuous filaments is preferably 120°C or higher and 180°C or lower. The lower limit of the melting point is more preferably 125°C or higher, even more preferably 130°C or higher, still more preferably 140°C or higher, and particularly preferably 145°C or higher. On the other hand, the upper limit of the melting point is more preferably 170°C or lower, even more preferably 160°C or lower. A melting point of 120°C or higher allows the heat treatment to be carried out within a suitable temperature range. On the other hand, a melting point of 180°C or lower improves flexibility, making it suitable for use as a cushioning material, etc.

[0055] The heat treatment time in the heat treatment step is preferably 1 minute or more. This can increase the melting enthalpy. The heat treatment time is more preferably 5 minutes or more, even more preferably 10 minutes or more, and particularly preferably 15 minutes or more. On the other hand, the upper limit of the heat treatment time in the heat treatment step is preferably 60 minutes or less, more preferably 50 minutes or less. This can reduce yellowing, odor, molecular weight reduction, etc. of the polybutylene adipate terephthalate resin that accompanies polymer decomposition and deterioration during heat treatment. Furthermore, productivity can also be improved.

[0056] The molded body cooled and solidified in the water bath is preferably held at a temperature of 20°C to 50°C for 1 minute or more (preferably 10 minutes or more, more preferably 30 minutes or more) before heat treatment. During heat treatment, the thickness of the molded body may change due to its own weight. However, by holding the molded body at a temperature of 20°C to 50°C after cooling and solidifying, it is possible to reduce the change in thickness of the molded body due to heat treatment. For example, after cooling and solidifying in the water bath, a continuous dryer may be used to hold the molded body at a low temperature in the first half of a hot air oven, and then the temperature of the hot air oven may be increased to perform heat treatment.

[0057] 1 and 2 are side views of a network structure manufacturing apparatus according to an embodiment of the present invention. The network structure manufacturing apparatus 1 includes a nozzle 10, a water tank 20, a conveying device 30, and a water discharge device 40 or 43. In the explanation of FIGS. 1 and 2, a three-dimensional network structure is sometimes referred to as a network structure. Note that FIG. 2 differs from FIG. 1 in that a water discharge device 43 is provided instead of the water discharge device 40. The apparatus of FIG. 1 is used in Examples 1 to 4 described below, and the apparatus of FIG. 2 is used in Example 5 described below.

[0058] The nozzle 10 has a discharge hole 11 through which the molten thermoplastic resin is extruded in the form of filaments. That is, the thermoplastic resin melted by heating is extruded from the discharge hole 11 of the nozzle 10 to form filaments of resin 12.

[0059] The discharge holes 11 of the nozzle 10 may be arranged in a single row, but are preferably arranged in multiple rows. By having multiple discharge holes 11 in the nozzle 10, multiple filaments of resin 12 can be formed simultaneously, thereby improving the production efficiency of the network structure 60. The number of discharge holes 11 in the nozzle 10 can be adjusted depending on the hardness and cushioning properties of the network structure 60 to be manufactured.

[0060] The cross-sectional shape of the filamentous resin 12 extruded from the discharge hole 11 may be solid or hollow. In order to make the cross-sectional shape of the filamentous resin 12 hollow, for example, a configuration having a mandrel portion such as a mandrel inside the discharge hole 11 may be used. Specifically, examples of such a nozzle include a so-called C-type nozzle in which the inside and outside of the discharge hole 11 are partially connected in cross section at the outlet of the discharge hole 11, and a so-called three-point bridge nozzle in which a bridge is provided in the discharge hole 11 to divide the discharge hole 11 in the circumferential direction.

[0061] The water tank 20 is disposed below the nozzle 10 and is configured to be able to receive the filamentous resin 12 extruded from the discharge holes 11 of the nozzle 10. The water tank 20 contains water for cooling the filamentous resin 12 extruded from the discharge holes 11 of the nozzle 10. The filamentous resin 12 extruded from the discharge holes 11 of the nozzle 10 hits the water surface in the water tank 20 and meanders to form random loops, which come into contact with adjacent random loops in a molten state, forming a structure in which the random loops are bonded together in three dimensions, and are simultaneously cooled by the water to fix the structure. In this manner, a network structure 60 is obtained.

[0062] The conveying device 30 is provided in the water tank 20 and conveys the network structure 60 having the filamentous resin 12. That is, the conveying device 30 conveys, within the water tank 20, the network structure 60 having the filamentous resin 12 that has been extruded from the discharge holes 11 of the nozzle 10 and received in the water tank 20. It is preferable that the conveying device 30 conveys the network structure 60 from the water surface of the water tank 20 toward the bottom of the water tank 20.

[0063] The conveying device 30 is composed of at least a first conveying device 31 and a second conveying device 32, and the network structure 60 is located between the first conveying device 31 and the second conveying device 32. By configuring the conveying device 30 in this manner, the network structure 60 can be conveyed while being sandwiched between the first conveying device 31 and the second conveying device 32, and therefore the network structure 60 can have a smooth surface and a uniform thickness.

[0064] As shown in FIG. 1 , the water discharge device 40 is provided above the conveying device 30 and discharges water in a predetermined direction. The network structure 60 between the conveying devices 30 does not exist on the extension of the water discharge direction of the water discharge device 40. In order to obtain a sufficient cooling rate difference, it is preferable that the water temperature difference between the water surface temperature of the water-receiving portion of the filament before the cooling water is discharged and the discharged cooling water be 5°C or more. If the water temperature difference is less than 5°C, a sufficient difference in the number of contact points may not be obtained. Furthermore, it is more preferable that the water temperature difference be 10°C or more. If the water temperature difference is less than 10°C, the temperature difference of the endothermic peak top appearing below the melting point may not be 1°C or more.

[0065] The amount of cooling water supplied from the top of the conveying device is preferably 0.04 L / min or more and 0.9 L / min or less per 1 cm of width of the conveying device. If it is less than 0.04 L / min, the resin cooling rate cannot be sufficiently improved. If it is more than 0.9 L / min, molding defects occur on the surface of the network structure, deteriorating the surface quality. Resin cooling can also be achieved by partially changing the speed of the cooling water. The water discharge device 40 is preferably positioned at a desired position in the network structure where the hardness is to be reduced in a band-like manner, and is preferably positioned 0.1 mm or more and 100 mm or less above the water surface in the water tank 20.

[0066] 2 includes a water discharge device 43 that discharges cooling water, and the position from which the cooling water is discharged by the water discharge device 43 is preferably below the water surface of the water tank 20. As shown in FIG. 1 , if the position from which the cooling water is discharged by the water discharge device 40 is above the water surface of the water tank 20, and the filaments of resin 12 extruded from the discharge holes 11 of the nozzles 10 come into contact with the cooling water discharged from the water discharge device 40 before landing in the cooling water in the water tank, the filaments of resin 12 may bend significantly, causing large irregularities on the surface of the network structure and poor formation. Therefore, if the position from which the cooling water is discharged by the water discharge device 40 is above the water surface of the water tank 20, it is necessary to adjust the angle of the cooling water discharged by the water discharge device 40, the angle of the discharge holes 11 of the nozzles 10, etc.

[0067] 2, if the position from which the cooling water is sprayed by the water discharge device 43 is below the water surface of the water tank 20, there is no risk that the filaments of resin 12 extruded from the discharge holes 11 of the nozzles 10 will come into contact with the cooling water sprayed from the water discharge device 43 before landing in the cooling water in the water tank, making it less likely that the formation of the network structure will deteriorate. Therefore, it is more preferable that the position from which the cooling water is sprayed by the water discharge device 43 is below the water surface of the water tank 20 than above it.

[0068] Fig. 3 is a schematic diagram of the network structure manufacturing apparatus 1 shown in Fig. 2 as viewed from above. Specifically, Fig. 3 is a schematic diagram of the first conveying device 31, the second conveying device 32, and the network structure 60 of the network structure manufacturing apparatus 1 as viewed from above. Note that the nozzles 10 and the discharge holes 11 are omitted from Fig. 3.

[0069] 3 , the water discharger 43 preferably sprays cooling water onto only a portion of the width of the first conveyor 31 and the second conveyor 32. The portions of the width of the first conveyor 31 and the second conveyor 32 can be rephrased as the portion of the width of the network structure 60 located between the first conveyor 31 and the second conveyor 32. By spraying cooling water onto only a portion of the width of the first conveyor 31 and the second conveyor 32, the cooling rate of the filamentary resin 12 that constitutes the network structure 60 can be partially changed by the cooling water sprayed from the water discharger 43.

[0070] The water discharge devices 40, 43 may be one or more. The amount of water discharged from the water discharge devices 40, 43 is preferably 0.6 L / min or more and 3.0 L / min or less per 1 cm of width of the water discharge device. The discharged water partially changes the water flow rate, making it possible to partially change the cooling rate of the thermoplastic elastomer. The cooling water jet position is preferably located 0.1 mm or more and 100 mm or less below the water surface in the water tank.

[0071] At any stage from the manufacturing process to the molding process of the thermoplastic resin used as the raw material for the three-dimensional network structure, additives capable of imparting functions such as deodorizing, antibacterial, antifungal, antimite, deodorizing, antifungal, aromatic, flame retardant, and moisture absorbing / releasing properties may be added to the thermoplastic resin. Furthermore, when manufacturing the three-dimensional network structure, the raw material polybutylene adipate terephthalate resin may contain function-imparting agents such as antioxidants and lubricants. These may be used alone or in combination of two or more. It is preferable to adjust the content of various function-imparting agents by kneading them into the resin during melt extrusion depending on the color tone and quality of the resin after melting.

[0072] Examples of the antioxidant include known phenol-based antioxidants, phosphite-based antioxidants, thioether-based antioxidants, benzotriazole-based ultraviolet absorbers, triazine-based ultraviolet absorbers, benzophenone-based ultraviolet absorbers, N—H type hindered amine-based light stabilizers, N—CH 3 and hindered amine-based light stabilizers. It is preferable that at least one of the above antioxidants is contained in the thermoplastic resin.

[0073] Examples of phenolic antioxidants include 1,3,5-tris[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 4,4'-butylidenebis(6-tert-butyl-m-cresol), 3-(3,5-di-tert-butyl-4-hydroxyphenyl)stearyl propionate, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], Sumilizer AG 80, and 2,4,6-tris(3',5'-di-tert-butyl-4'-hydroxybenzyl)mesitylene.

[0074] Examples of phosphite antioxidants include 3,9-bis(octadecyloxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, 2,4,8,10-tetrakis(1,1-dimethylethyl)-6-[(2-ethylhexyl)oxy]-12H-dibenzo[d,g]"1,3,2"dioxaphosphocin, tris(2,4-di-tert-butylphenyl) phosphite, tris(4-nonylphenyl) phosphite, and 4,4'-isopropylidenediphenol C12-15 alcohol. phosphite, diphenyl (2-ethylhexyl) phosphite, diphenyl isodecyl phosphite, triisodecyl phosphite, triphenyl phosphite, and the like.

[0075] Examples of the thioether antioxidant include 2,2-bis[3-(dodecylthio)propionic acid]3-(dodecylthio)-1-oxopropyloxymethyl]-1,3-propanediyl bis[3-(dodecylthio)propionic acid], ditridecyl 3,3'-thiobispropionate, and the like.

[0076] In order to prevent thermal degradation of the thermoplastic resin, a mixture of a phenolic antioxidant and a phosphite antioxidant may be used. When these two types of antioxidants are used, the total content of the two types of antioxidants is preferably 0.05% by mass or more and 1.0% by mass or less, based on 100% by mass of the thermoplastic resin composition.

[0077] Examples of the lubricant include hydrocarbon waxes, higher alcohol waxes, amide waxes, ester waxes, metal soap waxes, etc. If necessary, the lubricant is contained in an amount of preferably 0.5% by mass or less based on 100% by mass of the thermoplastic resin composition.

[0078] This application claims the benefit of priority based on Japanese Patent Application No. 2023-056166, filed on March 30, 2023. The entire contents of the specification of Japanese Patent Application No. 2023-056166, filed on March 30, 2023, are incorporated herein by reference.

[0079] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples. Furthermore, modifications can be made within the scope of the above and below-described aims, and all such modifications are within the technical scope of the present invention.

[0080] The characteristic values ​​of the three-dimensional network structures of Examples 1 to 5 and Comparative Examples 1 to 3 were measured according to the following methods. The sample sizes were standardized as described below, but when there were insufficient samples, measurements were performed using samples of the largest possible size.

[0081] (1) Absorbance Absorbance was measured using a SPECTROPHOTOMETER CM-3700d (manufactured by Konica Minolta, Inc.). A D65 light source was used, the viewing angle was set to 10°, the measurement range was set to a Φ8 mm circle, and reflected light was measured. For the measurement sample, the obtained three-dimensional network structure was cut into a length of 15 cm and a width of 15 cm, which was then cut into two pieces in the thickness direction, one of which was designated as side A and the other as side B. The sample of side A was cut into small pieces with scissors and then passed through a sieve with a mesh size of 2.8 mm. The piece that passed through was further passed through a sieve with a mesh size of 0.5 mm, and the piece remaining on the sieve was used. The size of the obtained sample (network piece) was 0.5 to 3 mm. 12.4±0.9 g of this was placed in a Φ38 mm cell, uniformly leveled, and sealed. This was used as a measurement sample, and the absorbance of side A was measured. The absorbance of side B was measured in the same manner as side A, and the difference in absorbance between side A and side B was calculated.

[0082] (2) Average Fiber Diameter The three-dimensional network structure was cut into pieces measuring 10 cm × 10 cm, and continuous filaments with a length of approximately 5 mm were collected from 10 locations on each piece. Next, an optical microscope was used to measure the diameter of the collected continuous filaments, with the focus adjusted to the location where the fiber diameter was to be measured, and the average value (n = 10) of the fiber diameters at the 10 locations was calculated.

[0083] (3) Hollowness Ten continuous filaments were randomly taken out from the three-dimensional network structure. The continuous filaments were then cut into cross sections, placed on a slide glass in a state where they were standing in the fiber axial direction, and the fiber cross sections in the cross section direction were observed under an optical microscope. In this case, only continuous filaments with hollow fiber cross sections were selected, and the area (a) within the outer circumferential line of the fiber and the area (b) of the hollow portion were calculated, respectively. The hollowness was calculated based on the following formula, and the average hollowness (n = 10) of the selected continuous filaments with hollow cross sections was determined. Hollowness (%) = (b) / (a) × 100

[0084] (4) Thickness and apparent density The three-dimensional network structure was cut into a size of 10 cm x 10 cm in the length and width directions, and the obtained sample was left unloaded for 24 hours. Thereafter, the height of one point at the center was measured using a test piece thickness measuring instrument (FD-80N type, manufactured by Kobunshi Keiki Co., Ltd.), and this height of the sample was taken as the thickness of the three-dimensional network structure. Furthermore, the sample was placed on an electronic balance and the weight of the sample was measured. The height of the sample and the area (100 cm) were used to measure the thickness of the three-dimensional network structure.2 The apparent density was calculated by dividing the weight of the sample by the volume. The above operation was repeated three times to calculate the average values ​​(n=3) of the thickness and apparent density of the three-dimensional network structure.

[0085] (5) Molar ratio of terephthalic acid units to adipic acid units of polybutylene adipate terephthalate resin The molar ratio of terephthalic acid units to adipic acid units of polybutylene adipate terephthalate resin is 1 Measurement was performed by H-NMR. The measurement device used was a BRUKER AVANCE-NEO600 NMR device, and the measurement was performed as follows. 10 to 15 mg of sample was dissolved in deuterated chloroform / trifluoroacetic acid = 85 / 15 (volume ratio), and the solution was then filled into an NMR tube and measurement was performed. Deuterated chloroform was used as the lock solvent, the waiting time was 1 second, the data acquisition time was 4 seconds, and the number of integrations was 64. When the chloroform peak is at 7.28 ppm, the adipic acid peak is detected at 2.45 ppm, and the terephthalic acid peak is detected at 8.15 ppm. When the peak integral value of adipic acid is A and the peak integral value of terephthalic acid is B, the molar ratio of terephthalic acid units to adipic acid units in polybutylene adipate terephthalate resin can be expressed by the following formula: Molar ratio = ((B / 4) ÷ (A / 4))

[0086] (6) 40°C Compression Set The three-dimensional network structure was cut into a size of 10 cm x 10 cm. Next, the thickness (c) of the obtained sample before treatment was measured using the method described in (4) above. The sample whose thickness had been measured was clamped between a jig capable of maintaining it in a 50% compressed state, placed in a dryer controlled at 40°C, and left for 22 hours. Thereafter, the sample was removed, cooled, and the compression set was removed. After leaving it for 30 minutes, the thickness (d) was calculated. These thicknesses were entered into the following formula to calculate the 40°C compression set. The above operation was performed three times, and the average value (n = 3) of the 40°C compression set was calculated. 40°C Compression Set (%) = ((c) - (d)) / (c) x 100

[0087] (7) 70°C Compression Residual Set The three-dimensional network structure was cut into a size of 10 cm x 10 cm. Next, the thickness (c) of the obtained sample before treatment was measured using the method described in (4) above. The sample whose thickness had been measured was clamped between a jig capable of maintaining it in a 50% compressed state, placed in a dryer controlled at 70°C, and left for 22 hours. Thereafter, the sample was removed, cooled, and the compression strain was removed. After leaving it for 30 minutes, the thickness (e) was calculated. These thicknesses were entered into the following formula to calculate the 70°C compression residual set. The above operation was performed three times, and the average value (n = 3) of the 70°C compression residual set was calculated. 70°C Compression Residual Set (%) = ((c) - (e)) / (c) x 100

[0088] (8) Hardness at 25% Compression The three-dimensional network structure was cut into a size of 30 cm x 30 cm, and the resulting sample was left in an environment of 23 ° C ± 2 ° C for 24 hours without load. Next, in an environment of 23 ° C ± 2 ° C, measurement was performed in accordance with ISO2439 (2008) E method using an autograph AG-X plus manufactured by Shimadzu Corporation. Specifically, a pressure plate with a diameter (φ) of 200 mm was placed at the center of the sample, and the thickness when the load reached 5 N was measured, which was defined as the initial thickness. The position of the pressure plate at this time was defined as the zero point, and pre-compression was performed once to 75% of the initial thickness at a speed of 100 mm / min. The pressure plate was then returned to the zero point at the same speed and left as is for 4 minutes. Thereafter, immediate compression was performed to 25% of the initial thickness at a speed of 100 mm / min. The load at this time was measured, and the weight was defined as the hardness at 25% compression (N / φ200 mm). The above procedure was repeated three times to determine the average value (n=3) of the hardness at 25% compression.

[0089] (9) Distinguishing between front and back The obtained samples were prepared, and five adult subjects visually judged whether they could distinguish between side A and side B. If three or more subjects were able to distinguish, it was judged as "distinguishable," and if three or more subjects were unable to distinguish, it was judged as "indistinguishable."

[0090] Polybutylene adipate terephthalate resin was synthesized by the following method. <Resin P> 1.5 mol of 1,4-butanediol, 0.40 mol of adipic acid, and 0.60 mol of dimethyl terephthalate were mixed in a reaction vessel equipped with a stirrer, thermometer, and distillation condenser. Next, 300 ppm of tetrabutyl titanate (manufactured by Aldrich) was added to the mixture as a titanium catalyst. Subsequently, transesterification and esterification reactions were carried out at 220°C under atmospheric pressure for 2 hours to prepare a prepolymer. The prepolymer was heated to 240°C and then subjected to a polycondensation reaction at 0.1 mmHg for 2 hours. The resulting Resin P was cooled and then cut into pellets using a pellet cutter. The melting point of Resin P was 150°C. The molar ratio of terephthalic acid units to adipic acid units in Resin P was 1.5.

[0091] [Example 1] Using resin P as a raw material, molten resin was extruded downward from a nozzle at a spinning temperature of 240°C and a single-hole extrusion rate of 3.87 g / min. The nozzle had an effective nozzle surface of 680 mm in width and 64 mm in thickness, and orifices with an outer diameter of 5.0 mm, an inner diameter of 4.4 mm, and a triple-bridge hollow-forming cross section were formed in a staggered arrangement with a hole pitch of 8 mm.

[0092] The water tank was arranged so that the water surface (hereinafter referred to as the water tank water surface) was located 31 cm below the nozzle surface of the nozzle for discharging the molten resin, and a pair of take-up conveyors were arranged in the water tank so that part of them was above the water surface. The water temperature in the water tank was 52 ° C. The take-up conveyor had a stainless steel endless net, and the conveyor was arranged parallel to the width direction of the nozzle surface, with the opening width of the endless net being 48 mm. In addition, to form the side portion (the two endless nets were considered to be the front and back portions), two aluminum plates were arranged 660 mm apart at a 90-degree angle relative to the net and the water surface to form the side portion.

[0093] The molten resin was extruded into the opening of the conveyor net (between the two endless nets), and the continuous filaments were dropped to form a meandering loop, fusing the contact portions to form a three-dimensional network structure. Both sides of the molten three-dimensional network structure were sandwiched between take-up conveyors, and while 14°C cooling water was sprayed from the outside of one of the conveyor nets at a rate of 0.45 L / min at a position 50 mm below the water surface, it was pulled below the water surface of the water tank at a speed of 2.32 m / min and solidified. This flattened both sides in the thickness direction and the lateral direction. It was then cut to a predetermined size and left to stand in a space at 25°C for 1 hour. It was then heat-treated with 90°C hot air for 20 minutes to obtain a three-dimensional network structure. The cross-sectional shape of the continuous filaments constituting the three-dimensional network structure was a hollow structure.

[0094] Example 2 A three-dimensional network structure was obtained in the same manner as in Example 1, except that a nozzle was used in which solid-forming orifices with an outer diameter of 1.0 mm were arranged in five rows at a hole pitch of 6 mm and further in nine rows of triple-bridge hollow-forming orifices with an outer diameter of 5 mm and an inner diameter of 4.4 mm at a hole pitch of 6 mm, the single-hole discharge rate was 1.35 g / min, the distance from the nozzle face to the water surface in the water tank was 25 cm, the take-up speed was 1.37 m / min, the water temperature in the water tank was 68°C, the cooling water was discharged from a position 35 mm below the water surface, and the cooling water temperature was 12°C.

[0095] Example 3 A three-dimensional network structure was obtained in the same manner as in Example 1, except that the spinning temperature was 220°C, the distance from the nozzle surface to the water surface in the water tank was 36 cm, the take-up speed was 1.91 m / min, the water temperature in the water tank was 55°C, the cooling water temperature was 12°C, and the cooling water discharge rate was 0.53 L / min.

[0096] Example 4 A three-dimensional network structure was obtained in the same manner as in Example 1, except that a nozzle was used in which round-hole orifices with an outer diameter of 1.0 mm were formed in a staggered arrangement with a hole pitch of 6 mm, the single-hole discharge rate was 1.50 g / min, the distance from the nozzle face to the water surface in the water tank was 20 cm, the take-up speed was 0.97 m / min, the water temperature in the water tank was 50°C, the cooling water discharge rate was 0.40 L / min, and the cooling water discharge position was 55 mm below the water surface in the water tank. The cross-sectional shape of the continuous filaments of the obtained three-dimensional network structure was round and had a solid structure.

[0097] Example 5 A three-dimensional network structure was obtained in the same manner as in Example 1, except that the single-hole discharge rate was 3.00 g / min, the distance from the nozzle surface to the water surface in the water tank was 28 cm, the water temperature in the water tank was 57°C, and instead of spraying cooling water at a position 50 mm below the water surface, cooling water at a temperature of 14°C was discharged at a rate of 0.10 L / min from a water discharge device provided 70 mm above one of the conveyor nets so as to contact the conveyor net, and the take-up speed was 1.57 m / min. However, the molten resin discharged from the nozzle was not present on the extension line of the discharged water, and the water discharged from the water discharge device was not directly hit on the continuous filaments.

[0098] Comparative Example 1 A three-dimensional network structure was obtained in the same manner as in Example 1, except that cooling water was not sprayed from the outside of the conveyor net when the three-dimensional network structure in the molten state was transported.

[0099] Comparative Example 2 A three-dimensional network structure was obtained in the same manner as in Example 3, except that cooling water was not sprayed from the outside of the conveyor net when the three-dimensional network structure in the molten state was transported.

[0100] Comparative Example 3 A three-dimensional network structure was obtained in the same manner as in Example 5, except that cooling water was not discharged from the water discharge device provided above the conveyor net when the three-dimensional network structure was formed.

[0101] The production conditions and the properties of the resulting three-dimensional network structures in Examples 1 to 5 and Comparative Examples 1 to 3 are shown in Table 1. In Table 1, the numerical values ​​of properties evaluated multiple times are average values.

[0102]

[0103] 1: Network structure manufacturing device 10: Nozzle 11: Discharge hole 12: Resin filaments 20: Water tank 30: Conveyor device 31: First conveyor device 32: Second conveyor device 40: Water discharge device 43: Water discharge device 60: Network structure

Claims

1. A three-dimensional mesh structure having a three-dimensional random loop joint structure composed of continuous filaments, wherein the thermoplastic resin composition constituting the continuous filaments contains 70% by mass or more of polybutylene adipate terephthalate, and the absolute value of the difference between the absorbance at a wavelength of 500 nm on one surface and the absorbance at a wavelength of 500 nm on the other surface on two opposing surfaces in the thickness direction of the three-dimensional mesh structure is 0.020 or more.

2. The three-dimensional network structure according to claim 1, wherein the polybutylene adipate terephthalate contains adipic acid units and terephthalic acid units, and the molar ratio of the terephthalic acid units to the adipic acid units is 0.8 or more and 3.0 or less.

3. The three-dimensional mesh structure according to claim 1 or 2, which is used as a cushioning material.

4. A method for producing the three-dimensional network structure according to claim 1 or 2, comprising: an extrusion process for extruding the molten thermoplastic resin composition from a nozzle; a molding process for obtaining a molded body having a three-dimensional network structure using the continuous filaments extruded from the nozzle; and a heat treatment process for heat treating the molded body, wherein the molding process comprises a step of immersing the continuous filaments in water in a water tank and a step of partially cooling the continuous filaments with a water discharge device, and the cooling water discharged from the water discharge device is at a temperature 5°C or more lower than that of the water in the water tank.

Citation Information

Patent Citations

  • Three-dimensional network structure and method for producing three-dimensional network structure

    JP2006097223A

  • Manufacturing method and manufacturing apparatus of three dimensional net-like structure

    JP2015155588A

  • Reticular structure manufacturing device and reticular structure manufacturing method

    WO2019188090A1

  • Biodegradable three-dimensional network structure

    WO2022209976A1