Polymer material and production thereof, and method for decomposing polymer material
The combination of a host group-containing polymer compound and a photoacid generator in the polymeric material allows for both high mechanical strength and easy decomposition, addressing the challenge of balancing toughness and degradability in polymeric materials.
Patent Information
- Application Number
- PCT/JP2024/011896
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-03
AI Technical Summary
There is a challenge in developing polymeric materials that balance mechanical toughness with ease of decomposition, as methods to enhance strength often result in low polymer molecular mobility, making it difficult for decomposing agents to effectively break down the material.
A polymeric material is created by combining a polymer compound with a host group, obtained from cyclodextrin or its derivatives, covalently bonded via a hemiaminal bond, and a photoacid generator, which allows for easy decomposition when irradiated with ultraviolet rays.
The material achieves a balance between mechanical toughness and degradability, enabling efficient decomposition while maintaining strength, and can be recycled effectively.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Polymer material, its production, and method for decomposing polymer material
[0001] The present invention relates to a polymeric material and a method for producing the same and for decomposing the polymeric material.
[0002] In recent years, the applications of polymeric materials have become increasingly diverse, and there is a demand for the creation of polymeric materials with various functions that can keep up with this diversification. For example, polymeric materials that have improved multiple physical properties that are in a so-called trade-off relationship, such as being hard yet having excellent extensibility, are expected to be applied in a variety of fields.
[0003] From this perspective, for example, Patent Document 1 proposes polymer materials having a reversible cross-linked structure utilizing host-guest interactions, polymer materials having a mobile cross-linked structure, etc. Such polymer materials have significantly improved mechanical properties such as toughness and strength, and are also capable of self-repairing, making them highly durable, and therefore they are expected to be applied to a variety of fields.
[0004] Japanese Patent Application Laid-Open No. 2021-181573
[0005] Meanwhile, in the field of polymeric materials, there is a strong demand for reducing environmental impacts. Therefore, polymeric materials that can be "extended in use" and "easily recovered as raw materials through decomposition" are desired. In other words, polymeric materials that are stable and durable during use and easily decompose after use or during recovery are desired. However, since there is generally a trade-off between the mechanical properties (strength, etc.) of polymeric materials and their decomposition efficiency, it is considered difficult to impart both toughness and easy decomposition properties to polymeric materials.
[0006] Specifically, to improve the strength of polymeric materials, methods such as strengthening the intermolecular interactions between polymer chains, forming crystals within the material, and introducing chemical crosslinks are generally considered. However, regardless of these methods, the resulting polymeric material has significantly low polymer molecular mobility. Therefore, even if a component (decomposer) that decomposes the polymeric material is added to the polymeric material, the decomposer is less likely to diffuse into the polymeric material, resulting in a decrease in the decomposition efficiency of the polymeric material. Although various decomposers exist for decomposing polymeric materials, their decomposition effect is limited when it comes to toughened polymeric materials, making it difficult to decompose them efficiently.
[0007] The present invention has been made in view of the above, and aims to provide a polymeric material that is strong yet easily decomposable, a method for producing the same, and a method for decomposing a polymeric material.
[0008] As a result of extensive research into achieving the above object, the inventors have discovered that the above object can be achieved by combining a polymer compound having a specific host group with a photoacid generator, and have thus completed the present invention.
[0009] That is, the present invention encompasses, for example, the subject matter described in the following items. Item 1: A polymer material comprising a polymer composition containing a polymer compound H and a photoacid generator, wherein the polymer compound H has at least one host group in the molecule, and the host group is a group obtained by removing at least one hydrogen atom or hydroxyl group from cyclodextrin or a cyclodextrin derivative, and the host group is covalently bonded to the polymer compound H via a hemiaminal bond. Item 2: A polymer material comprising a polymer composition containing a polymer compound H and a photoacid generator, wherein the polymer compound H has at least one host group in the molecule, and the host group is a group obtained by removing at least one hydrogen atom or hydroxyl group from cyclodextrin or a cyclodextrin derivative, and the host group is covalently bonded to the polymer compound H via a hemiaminal bond. 2 -NR b - (R b Item 3: The polymer material according to item 1, wherein the polymer compound H is a bond represented by the following general formula (1):
[0010] (In formula (1), R a represents a hydrogen atom or a methyl group, R brepresents hydrogen or an alkyl group, R H Item 4. The polymer material according to any one of Items 1 to 3, wherein the polymer compound H forms a crosslinked structure. Item 5. A method for producing the polymer material according to any one of Items 1 to 4, comprising the step of obtaining the polymer material by polymerization reaction of a raw material containing a monomer containing a polymerizable monomer having the host group and the photoacid generator. Item 6. A method for producing the polymer material according to any one of Items 1 to 4, comprising the step of obtaining the polymer material by mixing the polymer composition with the photoacid generator. Item 7. A method for decomposing the polymer material according to any one of Items 1 to 4, comprising the step of irradiating the polymer material with ultraviolet light. Item 9. A laminate comprising an adhesive layer containing the adhesive composition according to Item 8.
[0011] The polymer material of the present invention is a tough material, yet can be easily decomposed.
[0012] Schematic diagram of a crosslinked structure containing a polymer compound having a host group. UV-visible absorption spectrum of PAG. MALDI measurement results of Preliminary Test 2. (a) MALDI-TOF-MS spectrum of PAcγCD obtained in Production Example 1, (b) MALDI-TOF-MS spectrum of the dried product obtained in Test Example 1. Schematic diagram illustrating the cleavage of hemiaminal bonds in a polymer compound. USAXS-SAXS measurement results of the polymer material after ultraviolet irradiation in Test Example 1. Stretched SAXS measurement results of the polymer material after ultraviolet irradiation in Test Example 1. Results of mechanical properties obtained in Test Example 2. SEC measurement results after mercury lamp irradiation of a chloroform solution of the polymer material obtained in Example 3. Results of mechanical properties obtained in Test Examples 4-1 and 4-2. Results of mechanical properties obtained in Test Example 5. 1A is a schematic diagram showing the state of the tensile test carried out in Application Example 1, and FIG. 1B is a diagram showing the results of the mechanical properties measured in Application Example 1.
[0013]
[0023] In the present specification, the terms "contain" and "comprise" include the concepts of "contain," "comprise," "consist essentially of," and "consist only of."
[0014] The polymer material of the present invention contains a polymer composition containing a polymer compound H and a photoacid generator. In the polymer material of the present invention, the polymer compound H has at least one host group in the molecule, the host group being a group in which at least one hydrogen atom or hydroxyl group has been removed from cyclodextrin or a cyclodextrin derivative, and the host group is covalently bonded to the polymer compound H via a hemiaminal bond.
[0015] The polymer material of the present invention contains the polymer composition and a photoacid generator, and is therefore a tough material that can be easily decomposed.
[0016] (Polymer Compound H) The polymer material of the present invention contains, as an essential component, a polymer compound H having at least one host group. As described above, the host group is a group in which at least one hydrogen atom or hydroxyl group has been removed from a cyclodextrin or cyclodextrin derivative. The host group is not limited to a monovalent group; for example, the host group may be a divalent group, but is preferably monovalent in terms of ease of production.
[0017] The cyclodextrin derivative preferably has a structure in which the hydrogen atom of at least one of the hydroxyl groups of cyclodextrin is substituted with a hydrophobic group. In other words, the cyclodextrin derivative refers to a molecule having a structure in which a cyclodextrin molecule is substituted with another organic group having hydrophobic properties. However, the cyclodextrin derivative has at least one hydrogen atom or at least one hydroxyl group, preferably at least one hydroxyl group. The cyclodextrin derivative may be a cyclodextrin polymer, for example, a dimer. When the cyclodextrin derivative is a cyclodextrin polymer, the host group may be monovalent or may be divalent or higher.
[0018] The hydrophobic group is preferably a group substituted with at least one group selected from the group consisting of a hydrocarbon group, an acyl group, and -CONHR (R is a methyl group or an ethyl group). Hereinafter, in this specification, the aforementioned "at least one group selected from the group consisting of a hydrocarbon group, an acyl group, and -CONHR (R is a methyl group or an ethyl group)" may be referred to as a "hydrocarbon group, etc." for convenience.
[0019] Just to be clear, the term "cyclodextrin" used in this specification refers to at least one selected from the group consisting of α-cyclodextrin, β-cyclodextrin, and γ-cyclodextrin. Therefore, the cyclodextrin derivative is at least one selected from the group consisting of α-cyclodextrin derivatives, β-cyclodextrin derivatives, and γ-cyclodextrin derivatives.
[0020] The host group is a monovalent or higher group obtained by removing at least one hydrogen atom or hydroxyl group from a cyclodextrin or cyclodextrin derivative, and the hydrogen atom or hydroxyl group removed in the cyclodextrin derivative may be from any position on the cyclodextrin or cyclodextrin derivative. The host group is particularly preferably a monovalent group obtained by removing one hydrogen atom or hydroxyl group from a cyclodextrin or cyclodextrin derivative.
[0021] Here, when the total number of hydroxyl groups in one cyclodextrin molecule is N, N=18 for α-cyclodextrin, N=21 for β-cyclodextrin, and N=24 for γ-cyclodextrin.
[0022] If the host group is a monovalent group obtained by removing one "hydroxyl group" from a cyclodextrin derivative, the cyclodextrin derivative is formed by substituting the hydrogen atoms of up to N-1 hydroxyl groups per cyclodextrin molecule with hydrocarbon groups, etc. On the other hand, if the host group is a monovalent group obtained by removing one "hydrogen atom" from a cyclodextrin derivative, the cyclodextrin derivative can have the hydrogen atoms of up to N hydroxyl groups per cyclodextrin molecule substituted with hydrocarbon groups, etc.
[0023] The host group preferably has a structure in which the hydrogen atoms of 70% or more of the total number of hydroxyl groups present in one cyclodextrin molecule are substituted with the hydrocarbon group, etc. The host group more preferably has the hydrogen atoms of 80% or more of the total number of hydroxyl groups present in one cyclodextrin molecule substituted with the hydrocarbon group, etc., and particularly preferably has the hydrogen atoms of 90% or more of the total number of hydroxyl groups substituted with the hydrocarbon group, etc.
[0024] The host group preferably has a structure in which the hydrogen atoms of 13 or more of all the hydroxyl groups present in one α-cyclodextrin molecule are substituted with the hydrocarbon group, etc. The host group more preferably has the hydrogen atoms of 15 or more of all the hydroxyl groups present in one α-cyclodextrin molecule substituted with the hydrocarbon group, etc., and particularly preferably has the hydrogen atoms of 17 of all the hydroxyl groups substituted with the hydrocarbon group, etc.
[0025] The host group preferably has a structure in which the hydrogen atoms of 15 or more of all the hydroxyl groups present in one β-cyclodextrin molecule are substituted with the hydrocarbon group, etc. The host group more preferably has the hydrogen atoms of 17 or more of all the hydroxyl groups present in one β-cyclodextrin molecule substituted with the hydrocarbon group, etc., and particularly preferably has the hydrogen atoms of 19 or more of all the hydroxyl groups substituted with the hydrocarbon group, etc.
[0026] The host group preferably has a structure in which the hydrogen atoms of 17 or more of the total hydroxyl groups present in one γ-cyclodextrin molecule are substituted with the hydrocarbon group, etc. The host group more preferably has the hydrogen atoms of 19 or more of the total hydroxyl groups present in one γ-cyclodextrin molecule substituted with the hydrocarbon group, etc., and particularly preferably has the hydrogen atoms of 21 or more of the total hydroxyl groups substituted with the hydrocarbon group, etc.
[0027] In the cyclodextrin derivative, the type of the hydrocarbon group is not particularly limited, and examples of the hydrocarbon group include an alkyl group, an alkenyl group, and an alkynyl group.
[0028] The number of carbon atoms in the hydrocarbon group is not particularly limited, and the hydrocarbon group preferably has 1 to 4 carbon atoms, for example.
[0029] Specific examples of hydrocarbon groups having 1 to 4 carbon atoms include methyl, ethyl, n-propyl, isopropyl, and butyl. When the hydrocarbon group is a propyl or butyl group, it may be either linear or branched.
[0030] In the cyclodextrin derivative, examples of the acyl group include an acetyl group, a propionyl group, a formyl group, etc. The acyl group is preferably an acetyl group, in that it is easy to form a host-guest interaction, or other polymer chains can easily penetrate into the host group ring, and in that it is easy to obtain a polymer material excellent in toughness and strength.
[0031] In the cyclodextrin derivative, -CONHR (R is a methyl group or an ethyl group) is a methyl carbamate group or an ethyl carbamate group. -CONHR is preferably an ethyl carbamate group in that it is easy to form a host-guest interaction, or other polymer chains can easily penetrate into the host group ring, and it is easy to obtain a polymer material excellent in toughness and strength.
[0032] In the cyclodextrin derivative, the hydrocarbon group etc. is preferably an alkyl group or acyl group having 1 to 4 carbon atoms, more preferably a methyl group or an acyl group, more preferably a methyl group, an acetyl group or a propionyl group, and particularly preferably a methyl group or an acetyl group.
[0033] The structure of the polymer compound H is not particularly limited as long as it has at least one host group. For example, the host group can be covalently bonded to a side chain of the polymer compound H. Even in this case, the host group is covalently bonded to the side chain of the polymer compound H via a hemiaminal bond.
[0034] The hemiaminal bond is —O—CH 2 -NR b In this case, R b represents hydrogen or an alkyl group. b When R is an alkyl group, it has 1 to 20 carbon atoms, preferably 1 to 10 carbon atoms, more preferably 1 to 6 carbon atoms, and even more preferably 1 to 4 carbon atoms, and examples thereof include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, and a butyl group. The hydrocarbon group may be either linear or branched. Preferred R b is hydrogen, a methyl group, or an ethyl group, and more preferably R b is hydrogen or a methyl group, and more preferably R b is hydrogen.
[0035] Hemiaminal bond -O-CH 2 -NR b In the formula (I), the host group can be directly or indirectly bonded to the oxygen atom of the hemiaminal bond, and it is preferred that the host group is directly bonded to the oxygen atom of the hemiaminal bond.
[0036] The polymer compound H can have a host group-containing monomer unit. That is, the polymer compound H can be a polymer of a monomer containing a host group-containing polymerizable monomer. Therefore, the monomer unit means a repeating structural unit formed when the polymerizable monomer is polymerized.
[0037] The host group-containing polymerizable monomer is, for example, a compound having at least one (preferably one) host group and at least one (preferably one) polymerizable functional group, and the host group and the polymerizable functional group are separated by the hemiaminal bond.
[0038] The polymerizable functional group preferably has radical polymerizability, and examples thereof include a group containing a carbon-carbon double bond. Specific examples of the polymerizable functional group include an acryloyl group (CH 2 ═CH(CO)—), methacryloyl group (CH 2 = CCH 3 (CO)—), and other groups include a styryl group, a vinyl group, an allyl group, etc. These groups containing a carbon-carbon double bond may further have a substituent as long as the radical polymerizability is not inhibited.
[0039] The host group-containing polymerizable monomer may be, for example, a compound represented by the following general formula (1):
[0040]
[0041] In other words, the polymer compound H can have a structural unit based on the monomer represented by formula (1).
[0042] Here, in the formula (1), R a represents a hydrogen atom or a methyl group, R b represents hydrogen or an alkyl group, R H represents the host group. b is the aforementioned hemiaminal bond -O-CH 2 -NR b -R in b Therefore, in formula (1), R b When R is an alkyl group, it has 1 to 20 carbon atoms, preferably 1 to 10 carbon atoms, more preferably 1 to 6 carbon atoms, and even more preferably 1 to 4 carbon atoms, and examples thereof include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, and a butyl group. The hydrocarbon group may be either linear or branched. Preferred R b is hydrogen, a methyl group, or an ethyl group, and more preferably R b is hydrogen or a methyl group, and more preferably R b is hydrogen.
[0043] The host group R in the host group-containing polymerizable monomer represented by formula (1) His an example of a monovalent group obtained by removing one hydroxyl group from cyclodextrin or a derivative thereof. The host group-containing polymerizable monomer represented by formula (1) is a (meth)acrylamide derivative.
[0044] In this specification, "(meth)acrylic" means "acrylic" or "methacrylic", "(meth)acrylate" means "acrylate" or "methacrylate", and "(meth)allyl" means "allyl" or "methallyl".
[0045] As can be seen from the structural formula, the host group-containing polymerizable monomer represented by formula (1) has a structure in which a host group is directly bonded to the oxygen atom of the hemiaminal bond, and an acryloyl group or methacryloyl group is bonded to the nitrogen atom of the hemiaminal bond.
[0046] The method for producing the host group-containing polymerizable monomer is not particularly limited, and for example, a wide variety of known production methods can be employed.
[0047] Polymer compound H may have a monomer unit other than the host group-containing monomer unit. For example, polymer compound H may have a guest group-containing monomer unit. The guest group-containing monomer unit refers to a repeating structural unit formed when a guest group-containing polymerizable monomer is polymerized.
[0048] The guest group-containing polymerizable monomer is, for example, a compound having at least one (preferably one) guest group and at least one (preferably one) polymerizable functional group. The guest group-containing polymerizable monomer preferably does not have the hemiaminal bond.
[0049] The type of guest group is not limited as long as it is a group that can interact with the host group, particularly as long as it is a group that can be included in the host group. The guest group is not limited to a monovalent group, and may be, for example, a divalent group. Furthermore, the guest group-containing monomer unit may contain only one guest group, or may contain two or more guest groups.
[0050] Examples of the guest group include linear or branched hydrocarbon groups having 3 to 30 carbon atoms, cycloalkyl groups, heteroaryl groups, and organometallic complexes, which may have one or more substituents. Examples of the substituent are the same as those described above, and examples thereof include halogen atoms (e.g., fluorine, chlorine, bromine, etc.), hydroxyl groups, carboxyl groups, ester groups, amide groups, and optionally protected hydroxyl groups.
[0051] More specific examples of the guest group include linear or cyclic alkyl groups having 4 to 18 carbon atoms and groups derived from polycyclic aromatic hydrocarbons. The linear alkyl groups having 4 to 18 carbon atoms may be either linear or branched. The cyclic alkyl groups may have a cage structure. Examples of polycyclic aromatic hydrocarbons include π-conjugated compounds formed of at least two or more aromatic rings, and specific examples include naphthalene, anthracene, tetracene, pentacene, benzopyrene, chrysene, pyrene, and triphenylene.
[0052] Other examples of the guest group include monovalent groups formed by removing one atom (e.g., a hydrogen atom) from a guest molecule, such as at least one selected from the group consisting of alcohol derivatives; aryl compounds; carboxylic acid derivatives; amino derivatives; azobenzene derivatives having a cyclic alkyl group or a phenyl group; cinnamic acid derivatives; aromatic compounds and their alcohol derivatives; amine derivatives; ferrocene derivatives; azobenzene; naphthalene derivatives; anthracene derivatives; pyrene derivatives; perylene derivatives; clusters composed of carbon atoms such as fullerene; and dansyl compounds.
[0053] Further specific examples of the guest group include a t-butyl group, an n-octyl group, an n-dodecyl group, an isobornyl group, an adamantyl group, a group derived from pyrene, and groups in which the above-mentioned substituents are bonded to these groups.
[0054] The guest group-containing polymerizable monomer is not particularly limited as long as it is a compound having the guest group and polymerizability, and for example, a wide range of known guest group-containing polymerizable monomers can be exemplified. The guest group-containing polymerizable monomer preferably has a functional group having radical polymerizability. Examples of the functional group having radical polymerizability include a group containing a carbon-carbon double bond, and specifically, an acryloyl group (CH 2 ═CH(CO)—), methacryloyl group (CH 2 = CCH 3 (CO)—), and other groups include a styryl group, a vinyl group, an allyl group, etc. These groups containing a carbon-carbon double bond may further have a substituent as long as the radical polymerizability is not inhibited.
[0055] Specific examples of the guest group-containing polymerizable monomer include vinyl polymerizable monomers having the above-mentioned guest group. For example, the guest group-containing polymerizable monomer can be a compound represented by the following general formula (g1):
[0056]
[0057] In formula (g1), Ra represents a hydrogen atom or a methyl group, and R G represents the guest group, and R 2 represents a divalent group formed by removing one hydrogen atom from a monovalent group selected from the group consisting of a hydroxyl group, a thiol group, an alkoxy group which may have one or more substituents, a thioalkoxy group which may have one or more substituents, an alkyl group which may have one or more substituents, an amino group which may have one substituent, an amide group which may have one substituent, an aldehyde group, and a carboxyl group.
[0058] Among the polymerizable monomers represented by formula (g1), (meth)acrylic acid esters or derivatives thereof (i.e., R 2 is —COO—), (meth)acrylamide or a derivative thereof (i.e., R 2 is -CONH- or -CONR-, and R is the R bIn this case, the polymerization reaction proceeds easily, and the polymer compound H can be easily produced.
[0059] Specific examples of the guest group-containing polymerizable monomer include n-hexyl (meth)acrylate, n-octyl (meth)acrylate, n-dodecyl (meth)acrylate, adamantyl (meth)acrylate, hydroxyadamantyl (meth)acrylate, 1-(meth)acrylamidoadamantane, 2-ethyl-2-adamantyl (meth)acrylate, N-dodecyl (meth)acrylamide, t-butyl (meth)acrylate, 1-acrylamidoadamantane, N-(1-adamantyl)(meth)acrylamide, N-benzyl (meth)acrylamide, N-1-naphthylmethyl (meth)acrylamide, ethoxylated o-phenylphenol acrylate, phenoxy polyethylene glycol acrylate, isostearyl acrylate, nonylphenol EO adduct acrylate, isobornyl (meth)acrylate, (meth)acrylate having a pyrene moiety, and (meth)acrylamide having a pyrene moiety.
[0060] The guest group-containing polymerizable monomer can be produced by a known method. Alternatively, a commercially available guest group-containing polymerizable monomer can be used.
[0061] The polymer compound H may also have a monomer unit other than the host group-containing monomer unit and the guest group-containing monomer unit. Hereinafter, the monomer unit other than the host group-containing monomer unit and the guest group-containing monomer unit will be referred to as a "third monomer unit."
[0062] The third monomer unit refers to a repeating structural unit formed when a polymerizable monomer (third polymerizable monomer) copolymerizable with the host group-containing polymerizable monomer and the guest group-containing polymerizable monomer is polymerized. The third polymerizable monomer does not have the host group or the guest group. It is preferable that the third polymerizable monomer does not have the hemiaminal bond.
[0063] Examples of the third polymerizable monomer include various known vinyl polymerizable monomers. Specific examples of the third polymerizable monomer include compounds represented by the following general formula (a1):
[0064]
[0065] In formula (a1), Ra is a hydrogen atom or a methyl group, R 3 represents a halogen atom, a hydroxyl group, a thiol group, an amino group or a salt thereof which may have one substituent, a carboxyl group or a salt thereof which may have one substituent, an amide group or a salt thereof which may have one or more substituents, or a phenyl group which may have one or more substituents.
[0066] In formula (a1), R 3 is a carboxyl group having one substituent, examples thereof include a carboxyl group (i.e., an ester) in which the hydrogen atom of the carboxyl group has been substituted with a hydrocarbon group having 1 to 20 carbon atoms, a hydroxyalkyl group (for example, a hydroxymethyl group, a 1-hydroxyethyl group, or a 2-hydroxyethyl group), a methoxypolyethylene glycol (the number of ethylene glycol units is 1 to 20, preferably 1 to 10, and particularly preferably 2 to 5), or an ethoxypolyethylene glycol (the number of ethylene glycol units is 1 to 20, preferably 1 to 10, and particularly preferably 2 to 5). The hydrocarbon group having 1 to 20 carbon atoms preferably has 1 to 15 carbon atoms, more preferably 1 to 10, and particularly preferably 1 to 3 carbon atoms. The hydrocarbon group may be either linear or branched.
[0067] In formula (a1), R 3 is an amide group having one or more substituents, i.e., a secondary amide or a tertiary amide, examples of such a primary amide include amide groups in which one hydrogen atom or two hydrogen atoms of the primary amide are independently substituted with a hydrocarbon group or hydroxyalkyl group having 1 to 20 carbon atoms (e.g., a hydroxymethyl group, a 1-hydroxyethyl group, a 2-hydroxyethyl group). The hydrocarbon group having 1 to 20 carbon atoms preferably has 1 to 15 carbon atoms, and more preferably 2 to 10 carbon atoms. The hydrocarbon group may be either linear or branched.
[0068] Specific examples of the monomer represented by formula (a1) include (meth)acrylic acid, allylamine, maleic anhydride, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, n-octyl (meth)acrylate, (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethylacrylamide, N-isopropyl(meth)acrylamide, N-hydroxymethyl(meth)acrylamide, hydroxymethyl(meth)acrylate, 2-hydroxyethyl(meth)acrylamide, 2-hydroxyethyl(meth)acrylate, ethoxydiethylene glycol (meth)acrylate, methoxytriethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, and styrene. These may be used alone or in combination of two or more.
[0069] The third monomer unit is preferably (meth)acrylic acid, a (meth)acrylic acid ester, a (meth)acrylamide, or a derivative thereof, among the compounds represented by formula (a1). In this case, the polymerization reaction is likely to proceed, facilitating the production of polymer compound H.
[0070] As described above, in one embodiment, the polymer compound H contains a host group-containing monomer unit and, if necessary, may contain one or more monomer units selected from the group consisting of a guest group-containing monomer unit and a third monomer unit, and it is preferable that the polymer compound H contains at least both the host group-containing monomer unit and the third monomer unit.
[0071] Of all the structural units of polymer compound H, the content of the host group-containing monomer units is preferably 0.1 mol% or more, more preferably 0.3 mol% or more, even more preferably 0.5 mol% or more, and particularly preferably 1 mol% or more. Furthermore, of all the structural units of polymer compound H, the content of the host units is preferably 40 mol% or less, more preferably 20 mol% or less, even more preferably 10 mol% or less, and particularly preferably 5 mol% or less. In the present invention, the proportion (molar ratio) of each structural unit in polymer compound H can be considered to be the same as the molar ratio of each monomer used in producing the polymer compound.
[0072] The mass average molecular weight (Mw) of polymer compound H is not particularly limited, and can be, for example, 10,000 to 2,000,000, and preferably 20,000 to 1,000,000. Polymer compound H can be, for example, a random polymer, and can also be linear, and can also have a branched structure or a crosslinked structure as long as the effects of the present invention are not impaired.
[0073] The host group-containing monomer unit, the guest group-containing monomer unit and the third monomer unit contained in the polymer compound H may each be one type alone or two or more types.
[0074] The method for producing the polymer compound H is not particularly limited, and a wide variety of known production methods can be employed. For example, the polymer compound H can be produced by a polymerization reaction of a raw material containing the host group-containing polymerizable monomer and, if necessary, the guest group-containing monomer unit and / or the third polymerizable monomer. The polymerization reaction is also not particularly limited, and, for example, when the raw material contains a radical polymerizable monomer, a wide variety of known radical polymerization reactions can be applied.
[0075] More specific embodiments of polymer compound H include polymer compound H1, polymer compound H2, and polymer compound H3 shown below. Polymer compound H1: a polymer compound containing a host group-containing monomer unit, a guest group-containing monomer unit, and a third monomer unit. Polymer compound H2: a polymer compound containing a host group-containing monomer unit and a third monomer unit, but not a guest group-containing monomer unit. Polymer compound H3: a polymer compound containing a host group-containing monomer unit and a third monomer unit large enough to penetrate the host group.
[0076] <Polymer Compound H1> Polymer compound H1, which is one embodiment of polymer compound H, includes a host group-containing monomer unit, a guest group-containing monomer unit, and a third monomer unit.
[0077] In the polymer compound H1, the content of the guest group-containing monomer unit is preferably 0.1 mol % or more, more preferably 0.3 mol % or more, even more preferably 0.5 mol % or more, and particularly preferably 1 mol % or more, based on all the structural units of the polymer compound 1; and is preferably 40 mol % or less, more preferably 20 mol % or less, even more preferably 10 mol % or less, and particularly preferably 5 mol % or less.
[0078] In the polymer compound H1, the content of the third monomer unit is preferably 50 mol% or more, more preferably 70 mol% or more, even more preferably 80 mol% or more, and particularly preferably 90 mol% or more, based on all the structural units of the polymer compound H1; and is preferably 99.8 mol% or less, and more preferably 99 mol% or less.
[0079] In the polymer compound H1, the combination of the host group and the guest group is not particularly limited, and the host group and the guest group described above can be combined in any desired manner. In particular, when the host group is derived from α-cyclodextrin or a derivative thereof, the guest group is preferably at least one selected from the group consisting of an octyl group and a dodecyl group, as this facilitates the formation of the host-guest interaction described below and improves the mechanical properties of the polymer material. For the same reason, when the host group is derived from β-cyclodextrin or a derivative thereof, the guest group is preferably at least one selected from the group consisting of an adamantyl group and an isobornyl group, and when the host group is derived from γ-cyclodextrin or a derivative thereof, the guest group is preferably at least one selected from the group consisting of an octyl group, a dodecyl group, a cyclododecyl group, an adamantyl group, and a group derived from a polycyclic aromatic hydrocarbon. Examples of polycyclic aromatic hydrocarbons include pyrene.
[0080] The polymer compound H1 may be formed from only the host group-containing monomer unit, the guest group-containing monomer unit, and the third monomer unit.
[0081] <Polymer Compound H2> Polymer compound H2, which is one embodiment of polymer compound H, contains a host group-containing monomer unit and a third monomer unit, but does not contain a guest group-containing monomer unit.
[0082] The polymer compound H2 having such a structure can form a host-guest interaction with the guest group-containing polymer compound G described below. In the polymer compound H2, the third monomer unit preferably has a size that does not allow it to penetrate the host group.
[0083] The polymer compound H2 may be formed from only the host group-containing monomer unit and the third monomer unit.
[0084] <Polymer Compound H3> Polymer compound H3, which is one embodiment of polymer compound H, contains a host group-containing monomer unit and a third monomer unit having a size that allows it to penetrate the host group.
[0085] In the polymer compound H3, the third monomer unit having a size capable of penetrating the host group is preferably based on (meth)acrylic acid, a (meth)acrylic acid ester, (meth)acrylamide or a derivative thereof when the host group is derived from γ-cyclodextrin or a derivative thereof, and more preferably methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, or the like. In particular, when the host group is γ-cyclodextrin or a derivative thereof, ethyl (meth)acrylate is preferred.
[0086] The polymer compound H3 preferably does not contain a guest group-containing monomer unit, and the polymer compound H3 may also be formed only from a host group-containing monomer unit and a third monomer unit.
[0087] (Polymer composition) The polymer composition contained in the polymer material of the present invention contains at least the polymer compound H. The polymer composition may contain other polymer compounds in addition to the polymer compound H. Examples of other polymer compounds include a polymer compound containing a guest group and a chain polymer compound. Hereinafter, the polymer compound containing a guest group will be referred to as "polymer compound G" and the chain polymer compound will be referred to as "chain polymer compound P".
[0088] <Guest Group-Containing Polymer Compound G> The polymer compound G has the guest group-containing monomer unit and the third monomer unit in its molecule, but does not contain the host monomer unit. The guest group is bonded to the main chain or side chain of the polymer compound G by a covalent bond.
[0089] In terms of facilitating improvement in the mechanical properties of the polymer material and facilitating excellent flexibility, the content of the guest group-containing monomer unit in all the constituent units of the polymer compound G is preferably 0.1 mol% or more, more preferably 0.3 mol% or more, even more preferably 0.5 mol% or more, and particularly preferably 1 mol% or more, and is preferably 40 mol% or less, more preferably 20 mol% or less, even more preferably 10 mol% or less, and particularly preferably 5 mol% or less.
[0090] In terms of facilitating improvement in the mechanical properties of the polymer material and facilitating excellent flexibility, the content of the third monomer unit in all the constituent units of the polymer compound G is preferably 50 mol% or more, more preferably 70 mol% or more, even more preferably 80 mol% or more, particularly preferably 90 mol% or more, and is preferably 99.9 mol% or less, more preferably 99 mol% or less.
[0091] The polymer compound G may contain other monomer units (excluding the host unit) as long as the effects of the present invention are not impaired, or the polymer compound G may be formed only from the host unit and the third unit.
[0092] The mass average molecular weight (Mw) of the polymer compound G is not particularly limited, and can be, for example, 10,000 to 2,000,000, and preferably 20,000 to 1,000,000. The polymer compound G can be, for example, a random polymer, and can also be linear, and can also have a branched structure or a crosslinked structure, as long as the effects of the present invention are not impaired. The method for producing the polymer compound G is not particularly limited, and a wide variety of known production methods can be used.
[0093] When the polymer composition contains polymer compound G, the third units between polymer compound H and polymer compound G may be the same as each other, or may be partially or entirely different.
[0094] When the polymer composition contains polymer compound G, the combination of the host group in polymer compound H and the guest group in polymer compound G is not particularly limited, and the above-mentioned host groups and guest groups can be combined in any desired manner. In particular, when the host group is derived from α-cyclodextrin or a derivative thereof, the guest group is preferably at least one selected from the group consisting of an octyl group and a dodecyl group, in that the at least one host group in polymer compound H and the at least one guest group in polymer compound G are likely to improve the mechanical properties of the polymer material through host-guest interaction. For the same reason, when the host group is derived from β-cyclodextrin or a derivative thereof, the guest group is preferably at least one selected from the group consisting of an adamantyl group and an isobornyl group, and when the host group is derived from γ-cyclodextrin or a derivative thereof, the guest group is preferably at least one selected from the group consisting of an octyl group, a dodecyl group, a cyclododecyl group, an adamantyl group, and a group derived from the polycyclic aromatic hydrocarbon.
[0095] <Chain Polymer Compound P> The chain polymer compound P is, for example, a polymer compound having the third monomer unit and not having a host group. Among them, the chain polymer compound P is preferably a polymer of (meth)acrylic acid, a (meth)acrylic acid ester, (meth)acrylamide, or a derivative thereof, and more preferably a polymer of methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, or the like.
[0096] The chain polymer compound P may contain other monomer units (excluding host units and guest units) as long as the effects of the present invention are not impaired, or the chain polymer compound P may be formed solely from the third units.
[0097] The mass average molecular weight (Mw) of the chain polymer compound P is not particularly limited, and can be, for example, 10,000 to 2,000,000, and preferably 20,000 to 1,000,000. The chain polymer compound P can have a structure such as a homopolymer or a random polymer, and can be linear, and can also have a branched structure or a crosslinked structure as long as the effects of the present invention are not impaired.
[0098] There are no particular limitations on the method for producing the chain polymer compound P, and a wide variety of known production methods can be employed. For example, the chain polymer compound P can be produced by a polymerization reaction of a raw material containing the third polymerizable monomer. The polymerization reaction is also not particularly limited, and for example, when the raw material contains a radically polymerizable monomer, a wide variety of known radical polymerization reactions can be applied.
[0099] When the polymer composition contains a chain polymer compound P, the third units in the polymer compound H and the chain polymer compound P may be the same as each other, or some or all of them may be different.
[0100] <Form of polymer composition> In the polymer material of the present invention, the polymer compound H contained in the polymer composition preferably forms a crosslinked structure. In this case, the mechanical properties of the polymer material of the present invention are improved, and a tough material is likely to be formed. The crosslinked structure may be formed, for example, between polymer compounds H, or between polymer compound H and another polymer compound (for example, polymer compound G or chain polymer compound P).
[0101] The form of the polymer composition is not particularly limited as long as it contains polymer compound H. For example, the polymer composition may have the following forms such as polymer composition A, polymer composition B, polymer composition C, polymer composition D, polymer composition E, polymer composition F, and polymer composition G.
[0102] <Polymer Composition A> Polymer composition A, which is one embodiment of the polymer composition, contains the polymer compound H1 described above. Since polymer compound H1 has a host group and a guest group in its molecule, a host-guest interaction can be formed between the molecules. That is, at least one host group of the polymer compound H1 includes at least one guest group of another polymer compound H1, thereby forming an intermolecular host-guest interaction and forming a crosslinked structure of polymer compound H1.
[0103] Furthermore, such intermolecular host-guest interactions can also provide self-repairing properties. In this case, even if the polymer material is cut, the cut surfaces can be re-adhered, and the host-guest interaction is re-established at the adhesive surface, resulting in re-bonding and self-repair.
[0104] The polymer composition A may consist solely of the crosslinked structure of the polymer compound H1. The polymer composition A may further contain other polymer compounds as long as the effects of the present invention are not impaired.
[0105] The method for preparing the polymer composition A is not particularly limited, and for example, a wide variety of known methods can be employed. For example, a crosslinked structure of the polymer compound H1 can be formed by using an inclusion compound of a host group-containing polymerizable monomer and a guest group-polymerizable monomer and polymerizing the inclusion compound with a third polymerizable monomer, and the crosslinked structure can be used as the polymer composition A.
[0106] <Polymer Composition B> Polymer composition B, which is one embodiment of the polymer composition, contains the aforementioned polymer compound H2 and polymer compound G. In this case, the two polymer compounds can form an intermolecular host-guest interaction. That is, at least one guest group of polymer compound G is included in at least one host group of polymer compound H2, thereby forming an intermolecular host-guest interaction and forming a crosslinked structure of polymer compound H2, more specifically, a crosslinked structure between polymer compound H2 and polymer compound G. In addition, like polymer composition A, it can also have self-repairing properties.
[0107] The polymer composition B may consist only of a crosslinked structure of the polymer compound H2 and the polymer compound G. The polymer composition B may further contain other polymer compounds as long as the effects of the present invention are not impaired.
[0108] There are no particular limitations on the method for preparing the polymer composition B, and for example, a wide variety of known methods can be employed. For example, a crosslinked structure can be formed by mixing the polymer compound H2 with the polymer compound G, and this can be used as the polymer composition B.
[0109] <Polymer Composition C> Polymer composition C, which is one embodiment of the polymer composition, contains the above-mentioned polymer compound H2 and, if necessary, further contains the chain polymer compound P. When polymer composition C contains the chain polymer compound P, the chain polymer compound P can penetrate into the ring of the host group of polymer compound H2. This allows polymer compounds H2 to be crosslinked to each other by the chain polymer compound P to form a crosslinked structure, and in such a crosslinked structure, the chain polymer compound P can slide within the host group ring, making it possible to form a so-called mobile crosslinked structure.
[0110] Fig. 1(a) schematically shows a crosslinked structure (mobile crosslinked structure) in a polymer composition C, in which polymer compounds H2 having host groups h are crosslinked with each other by a chain polymer compound P. As shown in Fig. 1(a), the chain polymer compound P penetrates the host h group of the polymer compound H2, thereby crosslinking the polymer compounds H2 with each other by the chain polymer compound P and forming a mobile crosslinked structure. As a result, the mechanical properties of the polymer composition C are improved, and the polymer composition C can have excellent flexibility while being strong.
[0111] There are no particular limitations on the content ratio of the polymer compound H2 and the chain polymer compound P in the polymer composition C. For example, the content ratio of the host unit in the polymer compound H2 relative to the total amount of the structural units of both the polymer compound H2 and the chain polymer compound P is preferably 0.01 mol% or more, more preferably 0.1 mol% or more, even more preferably 0.3 mol% or more, and particularly preferably 0.5 mol% or more, and is preferably 40 mol% or less, more preferably 20 mol% or less, even more preferably 10 mol% or less, and particularly preferably 5 mol% or less.
[0112] In the polymer composition C, the third monomer unit in the polymer compound H2 preferably has a size that prevents it from penetrating into the ring of the host group of the polymer compound H2. Examples of the third polymerizable monomer for constituting such a third monomer unit include styrene, n-butyl(meth)acrylate, isobutyl(meth)acrylate, t-butyl(meth)acrylate, methoxyethyl(meth)acrylate, hexyl(meth)acrylate, 2-ethoxyhexyl(meth)acrylate, dodecyl(meth)acrylate, and polyethylene glycol(meth)acrylate.
[0113] In the polymer composition C, the chain polymer compound P is preferably a polymer of (meth)acrylic acid, a (meth)acrylic acid ester, (meth)acrylamide or a derivative thereof, and more preferably a polymer of methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, or the like.
[0114] The third monomer units are different in the polymer compound H2 and the chain polymer compound P. That is, the third monomer unit contained in the polymer compound H2 cannot penetrate the host group in the polymer compound H2, whereas the third monomer unit contained in the chain polymer compound P can penetrate the host group in the polymer compound H2.
[0115] The polymer composition C may consist only of a crosslinked structure of the polymer compound H2 and the chain polymer compound P. The polymer composition C may further contain other polymer compounds as long as the effects of the present invention are not impaired.
[0116] The polymer composition C can be prepared, for example, by the following method. First, a raw material (third monomer unit) for obtaining the chain polymer compound P is polymerized in the presence of the polymer compound H2 produced in advance. This polymerization reaction causes the propagation of the chain polymer compound P, and at the same time, the growing polymer chain can penetrate the host group. As a result, a mobile crosslinked structure composed of the polymer compound H2 and the chain polymer compound P is produced.
[0117] <Polymer Composition D> Polymer composition D, which is one embodiment of the polymer composition, contains the aforementioned polymer compound H3. In polymer composition D, at least one of the host groups possessed by polymer compound H3 is penetrated by the main chain of another polymer compound H3. The third monomer unit in polymer compound H3 has a size that allows it to penetrate into the ring of the host group possessed by polymer compound H3, so that the main chain of another polymer compound H3 can penetrate into the host group ring of polymer compound H3; more strictly, a segment composed of the third unit in another polymer compound H3 penetrates into the host group ring. As a result, in polymer composition D, a crosslinked structure (mobile crosslinked structure) between polymer compounds H3 is formed.
[0118] 1(b) is a schematic diagram showing a state in which another polymer compound H3 penetrates the host group h of the polymer compound H3. When another polymer compound H3 penetrates the host group of the polymer compound H3, a mobile crosslinked structure X is formed by the polymer compound H3, thereby improving the mechanical properties of the polymer material and providing it with toughness and excellent flexibility. Note that since the polymer compound Hc that penetrates the host group also has a host group, the host group acts as a so-called stopper and can prevent it from falling off.
[0119] The polymer composition D may consist solely of the polymer compound H3. The polymer composition D may further contain other polymer compounds as long as the effects of the present invention are not impaired.
[0120] The method for forming the mobile crosslinked structure of the polymer compound H3 is not particularly limited. For example, by carrying out a polymerization reaction for producing the polymer compound H3, the mobile crosslinked structure can be formed while the polymer compound H3 is being produced. Specifically, in the polymerization reaction of the polymer compound H3, as the propagation reaction of the polymer compound H3 progresses, the growing polymer chain penetrates the host group of another polymer chain, thereby forming the mobile crosslinked structure as shown in FIG. 1( b).
[0121] <Polymer Composition E> Polymer composition E, which is one embodiment of the polymer composition, contains the aforementioned polymer compound H3 and the chain polymer compound P. In polymer composition E, a mobile crosslinked structure is formed by polymer compound H3, similar to polymer composition D, and chain polymer compound P can be present in the mobile crosslinked structure. This can further improve the mechanical properties of the polymer material.
[0122] Fig. 1(c) is a schematic diagram showing the crosslinked structure of polymer composition E. As shown in Fig. 1(c), in polymer composition E, similarly to polymer composition D, a mobile crosslinked structure X is formed by a polymer compound H3 having a host group h, and a chain polymer compound P may be present penetrating the network of the crosslinked structure.
[0123] There are no particular limitations on the content ratio of the polymer compound H3 and the chain polymer compound P in the polymer composition E. For example, in terms of easily improving mechanical properties, the content ratio of the polymer compound H3 relative to the total mass of the polymer compound H3 and the chain polymer compound P can be, for example, 10% by mass or more, preferably 20% by mass or more, more preferably 40% by mass or more, and even more preferably 50% by mass or more, and can be 90% by mass or less, preferably 80% by mass or less, and more preferably 70% by mass or less.
[0124] The polymer composition E may consist only of the polymer compound H3 and the chain polymer compound P. The polymer composition E may further contain other polymer compounds as long as the effects of the present invention are not impaired.
[0125] There are no particular limitations on the method for producing the polymer composition E, and for example, a wide variety of known methods can be employed. For example, the polymer composition E can be prepared by carrying out a polymerization reaction to synthesize a chain polymer compound P in the presence of the polymer compound H3 that has been produced in advance to form a mobile crosslinked structure.
[0126] <Polymer Composition F> Polymer composition F, which is one embodiment of the polymer composition, contains a first polymer compound H3 and a second polymer compound H3. That is, polymer composition F contains at least two different types of polymer compounds H3.
[0127] In the polymer composition F, the third monomer units in the first polymer compound H3 and the second polymer compound H3 can both be (meth)acrylic acid ester units, for example. In this case, the (meth)acrylic acid ester units in the first polymer compound H3 and the second polymer compound H3 can be configured such that the number of carbon atoms in the alkyl groups of the alkyl ester moieties differ from each other. Specifically, a combination in which the (meth)acrylic acid ester unit in the first polymer compound H3 is methyl (meth)acrylate and the (meth)acrylic acid ester unit in the second polymer compound H3 is ethyl (meth)acrylate can be mentioned.
[0128] The polymer composition F contains a mobile cross-linked structure formed by a first polymer compound H3 and a mobile cross-linked structure formed by a second polymer compound H3. When the former mobile cross-linked structure is the first mobile cross-linked structure and the latter mobile cross-linked structure is the second mobile cross-linked structure, the mobile cross-linked structures can exist independently of each other, or can exist in a state where they are entangled with each other.
[0129] Fig. 1(d) is a schematic diagram showing the crosslinked structure of polymer composition F. As shown in Fig. 1(d), in polymer composition F, a mobile crosslinked structure X1 is formed by a first polymer compound H3(1) having a host group h, and a mobile crosslinked structure X2 is formed by a second polymer compound H3(2) having a host group h. The crosslinked structure X1 and the crosslinked structure X2 are present in a mutually entangled state.
[0130] (Photoacid Generator) The type of photoacid generator is not particularly limited as long as it is a compound that generates an acid by decomposition, for example, by ultraviolet light. Examples of the acid generated by the photoacid generator include sulfonic acids such as hydrochloric acid, methanesulfonic acid, ethanesulfonic acid, propanesulfonic acid, butanesulfonic acid, pentanesulfonic acid, octanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, camphorsulfonic acid, trifluoromethanesulfonic acid, p-phenolsulfonic acid, 2-naphthalenesulfonic acid, mesitylenesulfonic acid, p-xylene-2-sulfonic acid, m-xylene-2-sulfonic acid, 4-ethylbenzenesulfonic acid, 1H,1H,2H,2H-perfluorooctanesulfonic acid, perfluoro(2-ethoxyethane)sulfonic acid, pentafluoroethanesulfonic acid, nonafluorobutane-1-sulfonic acid, and dodecylbenzenesulfonic acid, as well as hydrates and salts thereof.
[0131] Specific examples of the photoacid generator include those disclosed in International Publication No. 2018 / 56281. Among these, bis(cyclohexylsulfonyl)diazomethane is a preferred photoacid generator. In these cases, the polymer material is likely to be decomposed by light irradiation, which makes it easier to recover raw materials.
[0132] The ultraviolet light for decomposing the photoacid generator preferably has a wavelength of, for example, 150 to 300 nm, and more preferably 200 to 250 nm.
[0133] (Polymer Material) The polymer material of the present invention contains a polymer composition containing polymer compound H and a photoacid generator. In the polymer material of the present invention, the content ratio of polymer compound H to photoacid generator is not particularly limited. For example, in order to facilitate decomposition of the polymer material, the content of the photoacid generator per 100 parts by mass of polymer compound H can be 0.1 parts by mass or more, preferably 1 part by mass or more, more preferably 25 parts by mass or more, even more preferably 50 parts by mass or more, and particularly preferably 100 parts by mass or more, and can be 500 parts by mass or less, preferably 450 parts by mass or less, more preferably 400 parts by mass or less, even more preferably 350 parts by mass or less, and particularly preferably 300 parts by mass or less.
[0134] The photoacid generator may be incorporated into a crosslinked structure containing polymer compound H, or may exist independently of the crosslinked structure. The photoacid generator may be unevenly distributed or uniformly distributed in the polymer material.
[0135] The polymer material may contain additives other than the polymer composition and the photoacid generator, as long as the effects of the present invention are not impaired. The polymer material may also be formed using only the polymer composition and the photoacid generator. The polymer composition and the photoacid generator may account for 50% by mass or more, preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 950% by mass or more, of the total amount of the polymer material.
[0136] The method for producing the polymer material is not particularly limited. For example, the polymer material of the present invention can be obtained by a production method including the following step A. Step A: A step of obtaining the polymer material by a polymerization reaction of a raw material containing a monomer containing a polymerizable monomer having a host group and the photoacid generator.
[0137] The production method including step A is a method in which a polymerization reaction of polymer compound H is carried out in the presence of the photoacid generator. In step A, the monomer containing a polymerizable monomer having a host group is, for example, a mixed monomer containing the above-mentioned host group-containing polymerizable monomer (e.g., a monomer represented by formula (1)). Such a mixed monomer can contain, for example, a predetermined amount of the guest group-containing polymerizable monomer and / or a third polymerizable monomer depending on the type of polymer composition.
[0138] When a photopolymerization initiator is used in the polymerization reaction of step A, it is preferable that the photopolymerization initiator has the property of initiating polymerization with ultraviolet light in a wavelength range in which the photoacid generator does not decompose. Specifically, the ultraviolet light that can be used in the polymerization reaction of step A preferably has a wavelength of 350 to 450 nm, more preferably 370 to 450 nm. It is preferable to use a photopolymerization initiator that can be used in this wavelength range in step A.
[0139] The polymer material of the present invention can be obtained by, for example, a method for producing a polymer material that includes the following step B. Step B: A step of obtaining the polymer material by mixing the polymer composition with the photoacid generator.
[0140] In the step B, the method for mixing the polymer composition and the photoacid generator is not particularly limited, and for example, the mixing treatment can be carried out using a known mixing means.
[0141] The polymer material of the present invention can be obtained by the production method including step A or step B as described above.
[0142] The polymer material of the present invention is a strong material having excellent mechanical properties and excellent toughness because it contains a polymer composition containing polymer compound H. In particular, when the polymer composition is any of the above-mentioned polymer compositions A, B, C, D, E, and F, the polymer material has particularly excellent toughness.
[0143] The form of the polymer material is not particularly limited, and may be, for example, a molded product such as a film, sheet, plate, or block, or may be in the form of particles, fibers, granules, pellets, or the like, or may be in a state dispersed or dissolved in a solvent.
[0144] When producing a molded article of a polymer material, the production method is not particularly limited, and for example, a wide variety of known molding methods can be adopted, such as a casting method, a press molding method, an extrusion molding method, and an injection molding method.
[0145] (Method for Decomposing Polymeric Materials) Since the polymeric material of the present invention contains a photoacid generator in addition to the polymer composition, the polymeric material can also be decomposed by irradiating the polymeric material with ultraviolet light. Specifically, when the polymeric material is irradiated with ultraviolet light, cleavage of the hemiaminal bond occurs. This causes the host group to separate from the polymer compound H, resulting in the elimination of the crosslinked structure formed by the polymer compound H, resulting in so-called decomposition of the polymeric material. This makes it possible to recover cyclodextrin or a derivative thereof derived from the host group from the polymeric material, or to recover the polymer component in the polymeric material.
[0146] For example, when the polymer compound H contained in the polymer material has a constitutional unit based on the monomer represented by the formula (1), when the hemiaminal bond site is cleaved, R H -OH(R H is a host group).
[0147] The method for recovering the host group-derived cyclodextrin or its derivative from the polymer material is not particularly limited. For example, a recovery method using a solvent can be preferably adopted, taking advantage of the phenomenon that dissolution or extraction into a solvent occurs easily when the crosslinked structure is eliminated. The type of solvent is not limited, and an appropriate organic solvent can be selected depending on the solubility of the polymer or cyclodextrin compound.
[0148] The method for decomposing the polymer material is not particularly limited. For example, the polymer material can be decomposed by a method including a step of irradiating the polymer material with ultraviolet light. As described above, the wavelength of the ultraviolet light is preferably 150 to 300 nm, and more preferably 200 to 250 nm. The duration of the ultraviolet light irradiation can be, for example, 30 to 90 minutes.
[0149] When decomposing a polymer material, moisture can be added. In this case, the decomposition of the polymer material is easily promoted, and the recovery efficiency can be further increased. For example, when decomposing a polymer material, the moisture content in the polymer material is preferably 3% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more, and is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 15% by mass or less, relative to the total mass of the polymer material.
[0150] When a polymer material contains moisture, the mechanical properties (e.g., the breaking stress of the polymer material) of the polymer after decomposition by UV irradiation are likely to decrease, which tends to increase the efficiency of recovering the cyclodextrin compound and polymer component from the polymer material.
[0151] Therefore, one aspect of the method for decomposing a polymeric material is to include a step of irradiating a polymeric material containing moisture with ultraviolet light. The method for adding moisture to the polymeric material is not particularly limited, and for example, a method of adding a predetermined amount of moisture to the polymeric material can be used.
[0152] Regardless of whether the polymer composition contained in the polymer material is any of the above-mentioned polymer compositions, it can be decomposed and has excellent recovery efficiency, but among them, polymer composition F is particularly excellent in recovery efficiency after decomposition of the polymer material.
[0153] The polymer material has excellent mechanical properties and also excellent decomposition performance, so that it can exhibit sufficient mechanical strength during use, and when it is no longer needed, it can be easily decomposed and various components can be recovered as needed. Therefore, the polymer material of the present invention can be used in various applications, and for example, the polymer material can be suitably used for various components for automobiles, electronic parts, building materials, food containers, transport containers, etc.
[0154] The excellent mechanical properties and degradability of polymeric materials make them suitable for use in adhesives, for example. Adhesives containing the polymeric material of the present invention can firmly bond adherends together. Furthermore, to break the bond, i.e., to separate the adherends, ultraviolet light can be applied. This causes the polymeric material to decompose, reducing the adhesive strength between the polymeric material and the adherend, facilitating separation.
[0155] Therefore, an adhesive composition can be prepared using the polymer material of the present invention, and such an adhesive composition containing the polymer material of the present invention can provide an adhesive layer that is excellent in adhesion and can be easily peeled off, which allows peeling without damaging the adherend, making it easy to reuse the adherend.
[0156] Various types of laminates can be formed using the adhesive layer formed from the adhesive composition. For example, a laminate can be formed by preparing a pair of adherends, forming an adhesive layer of the adhesive composition on one of the adherends, and then bonding the other adherend to this adhesive layer.
[0157] In specifying the inventions included in the present disclosure, the components (properties, structures, functions, etc.) described in each embodiment of the present disclosure may be combined in any manner. In other words, the present disclosure includes all subject matter consisting of all combinations of the components that can be combined as described in this specification.
[0158] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to these examples.
[0159] (Preparation Example 1) 5 g (3.9 mmol) of gamma cyclodextrin, 700 mg (6.9 mmol) of N-hydroxymethylacrylamide, and 95 mg (0.6 mmol) of p-toluenesulfonic acid monohydrate were weighed into a 200 mL glass round-bottom flask, and these were added to 25 mL of N,N-dimethylformamide to prepare a reaction solution. The solution was heated to 90°C in an oil bath and heated and stirred for 1 hour to obtain a reaction solution. The reaction solution was then allowed to cool and poured into 45 mL of vigorously stirred acetone. The resulting precipitate was filtered, washed three times with 10 mL of acetone, and dried under reduced pressure at room temperature for 1 hour to obtain a reaction product. The reaction product was dissolved in 100 mL of distilled water and passed through a column (apparent density 600 g / L) packed with porous polystyrene resin (Mitsubishi Chemical Diaion HP-20) and allowed to adsorb for 30 minutes. The solution components were then removed, and 50 mL of a 10% aqueous solution of methanol (or acetonitrile) was passed through the column three times to wash the polystyrene resin and remove unreacted γ-cyclodextrin. Next, 500 mL of a 25% aqueous solution of methanol was passed through the column twice to elute the target acrylamidomethyl γ-cyclodextrin (referred to as γCDAAmMe). The solvent was removed under reduced pressure to obtain γCDAAmMe as a white powder.
[0160] 20 g of this γCDAAmMe was dissolved in 300 mL of pyridine, and 170.133 g of acetic anhydride was added. The mixture was stirred at 55°C for 12 hours or more. Then, 50 mL of methanol was added to quench the mixture, and the mixture was concentrated in an evaporator until the internal volume reached 200 mL. The resulting concentrate was added dropwise to 2000 mL of water, and the precipitate was recovered. The precipitate was dissolved in 200 mL of acetone, and added dropwise to 2000 mL of water. The resulting precipitate was recovered and dried under reduced pressure to isolate the target host group-containing polymerizable monomer. The resulting host group-containing polymerizable monomer was a compound represented by the following formula (h1) (hereinafter referred to as "PAcγCD").
[0161]
[0162] Example 1: 0.03 mmol of 1-hydroxycyclohexyl phenyl ketone as a photopolymerization initiator was added to raw materials containing 0.06 mmol of PAcγCD obtained in Production Example 1 and 5.72 mmol of ethyl acrylate, and the mixture was subjected to ultrasonic irradiation for 1 minute to prepare a solution. Photopolymerization was carried out by irradiating the solution with ultraviolet light (wavelength 365 nm) for 2 hours. The polymer obtained by this polymerization was dried under reduced pressure at 60°C overnight, then immersed in 10 mL of chloroform, and then washed for 24 hours while replacing the chloroform several times. Next, the polymer was dried under reduced pressure at 40°C for 1 hour, and then dried under reduced pressure at 40°C overnight. This yielded polymer compound H having a host group. Polymer compound H formed the crosslinked structure (mobile crosslinked structure) shown in Figure 1(b).
[0163] The obtained polymer compound H was added to a chloroform solution prepared by dissolving 0.02 mmol of bis(cyclohexylsulfonyl)diazomethane (hereinafter referred to as PAG) as a photoacid generator in 10 mL of chloroform, thereby obtaining a polymer composition containing polymer compound H and a polymer material containing the photoacid generator.
[0164] Example 2 A solution was prepared by adding 0.06 mmol of 1-hydroxycyclohexyl phenyl ketone as a photopolymerization initiator and 0.05 mmol of PAG as a photoacid generator to a raw material containing 0.12 mmol of PAcγCD obtained in Production Example 1 and 12.83 mmol of ethyl acrylate, and then irradiating the mixture with ultrasonic waves for 1 minute. Photopolymerization was carried out by irradiating the solution with ultraviolet light (wavelength 365 nm) for 3.5 hours. This resulted in a polymer composition containing polymer compound H and a polymer material containing a photoacid generator. Polymer compound H formed the crosslinked structure (mobile crosslinked structure) shown in Figure 1(b).
[0165] Example 3: 0.03 mmol of 1-hydroxycyclohexyl phenyl ketone as a photopolymerization initiator was added to raw materials containing 0.06 mmol of PAcγCD obtained in Production Example 1 and 5.61 mmol of ethyl acrylate, and the mixture was ultrasonically irradiated for 5 minutes to prepare a solution. Photopolymerization was carried out by irradiating the solution with ultraviolet light (wavelength 365 nm) for 2 hours. The polymer obtained by this polymerization was cut into 1 / 8ths of its original size, and the resulting sample was immersed in 5 mL of chloroform. The sample was then washed for 40 hours, with the chloroform replaced several times. The sample was then dried under reduced pressure at 40°C for 6 hours, and then dried overnight at 40°C. The mass of the washed sample was measured, and the amount of PAcγCD was estimated from the charge ratio. A chloroform solution was prepared by weighing out PAG equivalent to the amount of PAcγCD and dissolving it in 3 mL of chloroform. The washed sample was then added to the chloroform solution. This resulted in a polymer material containing a polymer composition containing polymer compound H and a photoacid generator. The polymer compound H formed a crosslinked structure (mobile crosslinked structure) shown in FIG. 1(b).
[0166] Example 4 A mixed monomer of PAcγCD obtained in Production Example 1, methyl methacrylate (MMA), and ethyl acrylate (EA) was prepared. The molar ratio of the mixed monomers, PAcγCD:MMA:EA, was 1:24.6:74.4. 1-hydroxycyclohexyl phenyl ketone as a photopolymerization initiator and PAG as a photoacid generator were added to this mixed monomer, and the mixture was subjected to ultrasonic irradiation for 1 minute to prepare a solution. The photopolymerization initiator and photoacid generator added to the solution were 0.5 mol % relative to the mixed monomers, and 1 mol % relative to the mixed monomers. The solution was photopolymerized by irradiating with ultraviolet light (wavelength 365 nm) for 2 hours, followed by drying under reduced pressure at 60°C overnight. This resulted in a polymer composition containing polymer compound H and a polymer material containing a photoacid generator. Polymer compound H formed the crosslinked structure (mobile crosslinked structure) shown in Figure 1(b).
[0167] Example 5 A mixed monomer 1 was prepared from the PAcγCD obtained in Production Example 1 and ethyl acrylate (EA). The molar ratio of PAcγCD:EA in the mixed monomer 1 was set to 1.01:98.99. 1-Hydroxycyclohexylphenyl ketone was added to this mixed monomer 1 as a photopolymerization initiator, and the mixture was subjected to ultrasonic irradiation for 1 minute to prepare a solution. The amount of photopolymerization initiator added to the solution was 0.5 mol% relative to the mixed monomer 1. The solution was photopolymerized by irradiating it with ultraviolet light (wavelength 365 nm) for 2 hours, and then dried overnight under reduced pressure at 60°C. This yielded the crosslinked structure (mobile crosslinked structure) shown in Figure 1(b). This crosslinked structure was designated as mobile crosslinked structure X1.
[0168] Meanwhile, mixed monomer 2 was prepared from the PAcγCD obtained in Production Example 1 and methyl methacrylate (MMA). The molar ratio of PAcγCD:MMA in mixed monomer 2 was 1:99. To this mixed monomer 2, 1-hydroxycyclohexyl phenyl ketone as a photopolymerization initiator, PAG as a photoacid generator, and chloroform as a solvent were added, and ultrasonic irradiation was performed for 1 minute to prepare a chloroform solution. The photopolymerization initiator added to the chloroform solution was 0.5 mol % relative to mixed monomer 2, the photoacid generator was 2.5 mol % relative to mixed monomer 2, and the chloroform was added in an amount approximately 1.5 times the mass of mixed monomer 2. The mobile crosslinked structure X1 was immersed in this chloroform solution overnight, and then dried in a windy oven at 40°C for 1 hour. The chloroform was then dried to obtain a dried product. This dried product was irradiated with ultraviolet light (wavelength 365 nm) for 2 hours to cause photopolymerization, thereby producing the crosslinked structure (mobile crosslinked structure) shown in FIG. 1( b). As a result, a polymer material containing a polymer composition having the structure shown in FIG. 1( d) and a photoacid generator was obtained.
[0169] (Preliminary Test 1) As a preliminary test, ultraviolet-visible absorption spectrum of PAG (Bis(cyclohexylsulfonyl)diazomethane), a photoacid generator, was measured to examine the PAG absorption wavelength.
[0170] FIG. 2 is the UV-visible absorption spectrum of PAG.
[0171] (Preliminary Test 2) The effect of PAG on only the PAcγCD obtained in Production Example 1 was investigated in advance. Specifically, 0.05 mmol of PAcγCD obtained in Production Example 1 and 0.05 mmol of PAG were dissolved in 2 mL of chloroform to prepare a solution. This solution was irradiated with ultraviolet light (white light (mercury lamp) with peaks at wavelengths λ=253 and 365 nm) for 1 hour. Thereafter, the solution was air-dried in a fume hood to remove the chloroform, and the molecular weight was measured using a MALDI-TOF-MS spectrum.
[0172] Figure 3 shows the results of MALDI measurement in Preliminary Test 2. The upper spectrum in Figure 3 is the MALDI-TOF-MS spectrum of the solution before UV irradiation, and the lower spectrum is the MALDI-TOF-MS spectrum of the solution after UV irradiation. After UV irradiation, the spectrum specific to PAcγCD observed before UV irradiation disappeared, and instead, a spectrum due to partial decomposition products of hemiaminal clearly appeared. In other words, it was found that the hemiaminal bond in PAcγCD was cleaved. From these results, it was found that PAG has the ability to cleave the hemiaminal bond in PAcγCD. It is presumed that cleavage of the hemiaminal bond in PAcγCD converts the hemiaminal oxygen to a hydroxyl group. Therefore, for example, it is presumed that PAcγCD changes to a structure represented by the following formula (h1-1):
[0173]
[0174] (Test Example 1) A chloroform solution of the polymer material obtained in Example 1 was irradiated with ultraviolet light (white light (mercury lamp) having peaks at wavelengths λ of 253 and 365 nm) for 1.5 hours, and then the chloroform solution was air-dried in a draft to obtain a dried product. The molecular weight of the obtained dried product was measured using the MALDI-TOF-MS spectrum.
[0175] Figure 4(b) shows the MALDI-TOF-MS spectrum of the dried product obtained in Test Example 1. For comparison, Figure 4(a) shows the MALDI-TOF-MS spectrum of PAcγCD obtained in Production Example 1. Based on the spectral results in Figures 4(a) and 4(b) and the MALDI measurement results of Preliminary Test 2 (Figure 3), it is presumed that the ultraviolet irradiation performed in Test Example 1 cleaved the hemiaminal bond in polymer compound H, converting the hemiaminal oxygen to a hydroxyl group (i.e., it is presumed that the compound represented by (h1-1) above was produced). This demonstrates that the presence of a photoacid generator in a polymer material can cause acid decomposition of the hemiaminal bond.
[0176] Fig. 5 is a schematic diagram showing how the hemiaminal bond in polymer compound H is cleaved. In Fig. 5, h represents a host group, and X1 represents a crosslinked structure.
[0177] (Test Example 1a: Recovery of Raw Materials) In Test Example 1, the polymeric material after UV irradiation was washed with chloroform, and the residue after drying the washings was subjected to GPC measurement. It was found that the residue contained a compound in which the oxygen in the hemiaminal bond in PAcγCD had been converted to a hydroxyl group (i.e., the compound represented by (h1-1) above). The recovery rate was 13%. This demonstrates that compounds derived from the raw materials of the polymeric material can be recovered by irradiating the polymeric material with UV light.
[0178] (Test Example 1b: Physical Properties After Acid Decomposition) Fig. 6 shows the results of USAXS-SAXS measurement of the polymer material after ultraviolet irradiation in Test Example 1. In this measurement, the USAXS and SAXS profiles were measured at q = 0.06 nm -1 The results in Figure 6 suggest the possibility of the formation of structures of a certain size after photolysis.
[0179] Figure 7 shows the results of stretching SAXS measurement of the polymer material after UV irradiation in Test Example 1. Figure 7(a) shows the result before UV irradiation, and (b) shows the result after UV irradiation. In both (a) and (b), the graphs on the left show the SAXS measurement in the stretching direction, and the graphs on the right show the SAXS measurement in the perpendicular direction. The results in Figure 7 suggest that stretch orientation may be easier after UV irradiation. This is presumably due to cleavage of crosslinking points.
[0180] (Test Example 2) The polymer material obtained in Example 2 was cut in half, and one half was irradiated with ultraviolet light (white light (mercury lamp) having peaks at wavelengths λ=253 and 365 nm) for 1.5 hours, and then its mechanical properties were evaluated. The other half of the polymer material was not irradiated with ultraviolet light, and its mechanical properties were evaluated for comparison.
[0181] Figure 8 shows the results of the mechanical properties measured in Test Example 2. Figure 8(a) is a graph showing the relationship between Young's modulus and fracture energy, and Figure 8(b) is a graph showing the relationship between strain and stress. In Figure 8, "Before" is before ultraviolet irradiation, and "After" is after ultraviolet irradiation.
[0182] 8, it was found that both Young's modulus and toughness (fracture energy) decreased with UV irradiation. This result supports the idea that UV irradiation of a polymeric material containing PAG causes an acid decomposition reaction in the elastomer, cleaving hemiaminal bonds and reducing the number of crosslinking points.
[0183] (Test Example 3) A chloroform solution of the polymer material obtained in Example 3 was irradiated with white light from a mercury lamp (wavelength: λ = 253 and 365 nm peaks) for 90 minutes. After irradiation, the solution was dried for 6 hours using a blower at 40°C. 1.5 mL of DMSO was then added to the dried product, and the mixture was shaken for 30 minutes to prepare a DMSO solution. SEC measurement was then performed using the DMSO solution.
[0184] Figure 9 shows the results of SEC measurement. From this SEC, a peak identical to the peak due to the compound represented by (h1-1) (represented as "1" in Figure 9) was observed in the chloroform solution irradiated with the mercury lamp (represented as "AcγCD" in Figure 9). On the other hand, no peak due to the compound represented by (h1-1) was observed in the chloroform solution not irradiated with the mercury lamp (represented as "2" in Figure 9). Therefore, it was found that the compound represented by (h1-1) was produced by irradiating a polymer material containing PAG with ultraviolet light.
[0185] (Test Example 4-1) The polymer material obtained in Example 4 was cut in half to prepare a pair of polymer materials. Each polymer material was wrapped in water-soaked Kimwipe and left in a sealed container for about two days to absorb water. After absorbing water, the polymer material turned cloudy. Thereafter, one of the polymer materials was irradiated with ultraviolet light (white light (mercury lamp) with peaks at wavelengths λ = 253 and 365 nm) for 1.5 hours. After irradiation, the mechanical properties of the polymer material were evaluated. The other polymer material was not irradiated with ultraviolet light, and its mechanical properties were evaluated for comparison.
[0186] (Test Example 4-2) The polymer material obtained in Example 4 was cut in half to prepare a pair of polymer materials. One of the polymer materials was irradiated with ultraviolet light (white light (mercury lamp) having peaks at wavelengths λ=253 and 365 nm) for 1.5 hours. After irradiation, the mechanical properties of the polymer material were evaluated. The other polymer material was not irradiated with ultraviolet light, and its mechanical properties were evaluated for comparison.
[0187] Fig. 10 shows the results of the mechanical properties measured in Test Examples 4-1 and 4-2. Specifically, Fig. 10(a) and (b) show the results of Test Example 4-2, and Fig. 10(c) and (d) show the results of Test Example 4-1.
[0188] From Figure 10, it can be seen that in the case of a polymeric material containing water (Test Example 4-1, Figures 10(c) and (d)), ultraviolet irradiation (UV irradiation) reduces the Young's modulus and the mechanical strength. This result indicates that adding water to a polymeric material and irradiating it with ultraviolet rays makes the polymeric material more easily decomposed. Therefore, it can be said that the water present in the polymeric material has the effect of promoting the decomposition of the polymeric material, and it is presumed that this makes the recovery and decomposition process easier.
[0189] Test Example 5 The polymer material obtained in Example 5 was irradiated with a mercury lamp for 90 minutes, and then the sample and an unirradiated sample were evaluated by a tensile test.
[0190] FIG. 11 shows the results of the mechanical properties obtained in Test Example 5. Specifically, FIG. 11 shows that the Young's modulus of the polymer material obtained in Example 5 decreases upon ultraviolet irradiation (UV irradiation), and that the mechanical strength also decreases. This result, unlike FIG. 10, indicates that the polymer material is easily decomposed by ultraviolet irradiation even without adding water to the polymer material. Therefore, it is presumed that the recovery and decomposition process of the polymer material obtained in Example 5 becomes easier upon ultraviolet irradiation.
[0191] (Application Example 1) An adhesion test was performed using the method shown in Figure 12(a). First, a mixed monomer of PAcγCD obtained in Production Example 1 and ethyl acrylate (EA) was prepared. The molar ratio of the mixed monomers, PAcγCD:EA, was set to 1:99. 1-hydroxycyclohexyl phenyl ketone as a photopolymerization initiator and PAG as a photoacid generator were added to this mixed monomer, and the mixture was subjected to ultrasonic irradiation for 1 minute to prepare a solution. The photopolymerization initiator added to the solution was 0.5 mol% relative to the mixed monomer, and the photoacid generator was 1 mol% relative to the mixed monomer.
[0192] Separately, a pair of rectangular 6,10-nylon substrates was prepared, and their surfaces were plasma-treated. The vinyl groups were then modified with a silane coupling agent to prepare a pair of adherends S1 and S2. On the silane coupling agent-treated surface of one of the adherends S1, an area 1.5 cm from one end was designated as adhesive zone A1. 25 μL of the solution was applied to the entire surface of adhesive zone 50 to form a coating film M. The adhesive zone A2 of the other adherend S2 was then placed on top of this coating film M, and adherend S2 was bonded to adherend S1 so that the surfaces other than adhesive zone A2 did not overlap with adherend S1, forming a laminate. The coating film M in this laminate was photopolymerized by irradiating it with ultraviolet light (wavelength 365 nm) for 2 hours, curing the coating film M and bonding the adherends together. The cured coating film M (adhesive layer M) was then irradiated with a mercury lamp for 90 minutes, after which a tensile test of the laminate was performed. All of the above operations were carried out three times in total.
[0193] As shown in Figure 12(a), in the tensile test of the laminate, the adherends S1 and S2 were pulled in the 180° direction until the coating film broke, and the pulling distance x (mm) at the time of break was measured. The value obtained by dividing this x by the thickness y (mm) of the coating film was defined as the shear strain (x / y).
[0194] FIG. 12(b) shows the results of a tensile test conducted in Application Example 1. Specifically, it is a graph showing the stress at break (average of three tests) after irradiation with a mercury lamp. For comparison, FIG. 12(b) also shows the results of a tensile test without irradiation with a mercury lamp. The results in FIG. 12(b) demonstrate that irradiation with a mercury lamp can reduce the stress at break. This result demonstrates that irradiating an adhesive (adhesive layer) formed from the polymer material of the present invention with a mercury lamp can weaken the adhesive strength between bonded adherends. Therefore, when the polymer material of the present invention is used as an adhesive, the bonded adherends can be easily peeled from each other.
[0195] (Method for evaluating mechanical properties) The mechanical properties of the polymeric material were evaluated by observing the breaking point of the polymeric material through a tensile test (stroke-test force curve) (Shimadzu Corporation's "AUTOGRAPH" (model number: AGX-plus)). This breaking point was taken as the end point, and the maximum stress up to the end point was taken as the breaking stress of the polymeric material. This tensile test was carried out using an up-type method in which the polymeric material was punched into the shape of a dumbbell test piece with a thickness of 0.76 mm, the lower end was fixed, and the upper end was moved at a tensile speed of 1 mm / min or 5 mm / min. The test was carried out. The stroke at that time, i.e., the maximum length when the polymer material was pulled, divided by the length of the polymer material before pulling, was calculated as the strain rate. In the "stroke-test force curve" (stress-strain curve) test, a material that shows high values for either or both of the breaking stress and breaking strain (also simply referred to as strain) can be determined to have excellent toughness and strength. In particular, a material that shows high values for both the breaking stress and strain can be determined to have excellent fracture energy.
Claims
1. A polymer material comprising a polymer composition containing a polymer compound H and a photoacid generator, said polymer compound H having at least one host group in the molecule, said host group being a group in which at least one hydrogen atom or hydroxyl group has been removed from a cyclodextrin or a cyclodextrin derivative, said host group being covalently bonded to said polymer compound H via a hemiaminal bond.
2. The hemiaminal bond is —O—CH 2 -NR b - (R b The polymer material according to claim 1 , wherein R is a bond represented by the formula (I) in which R represents hydrogen or an alkyl group.
3. The polymer compound H is represented by the following general formula (1): (In formula (1), R a represents a hydrogen atom or a methyl group, R b represents hydrogen or an alkyl group; R H The polymer material according to claim 1 , comprising a structural unit based on a monomer represented by the following formula:
4. The polymer material according to claim 1, wherein the polymer compound H forms a crosslinked structure.
5. A method for producing a polymeric material according to any one of claims 1 to 4, comprising a step of obtaining the polymeric material by a polymerization reaction of a raw material containing a monomer containing a polymerizable monomer having a host group and the photoacid generator.
6. A method for producing a polymeric material according to any one of claims 1 to 4, comprising the step of obtaining the polymeric material by mixing the polymer composition with the photoacid generator.
7. A method for decomposing a polymeric material according to any one of claims 1 to 4, comprising the step of irradiating the polymeric material with ultraviolet light.
8. An adhesive composition comprising the polymer material according to any one of claims 1 to 4.
9. A laminate comprising an adhesive layer containing the adhesive composition according to claim 8.
Citation Information
Patent Citations
Adhesive composition
JP2022144831A
Inclusion complex, photoresist composition having the inclusion complex and method of forming a pattern using the photoresist composition
US20080070155A1
Host-group-containing polymerizable monomer, polymer material, method for producing same, and clathrate compound and method for producing same
WO2018159791A1