Resin composition, cured product, laminate, semiconductor device, and method for producing semiconductor device

The resin composition addresses the stability and adhesion issues in semiconductor devices by incorporating specific structural units and a silane coupling agent, ensuring reliable adhesion and heat resistance for ultra-thin semiconductor devices.

WO2024204181A1PCT designated stage expired Publication Date: 2024-10-03TORAY INDUSTRIES INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011922
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-26
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing resin compositions for semiconductor devices face challenges such as low dimensional stability, warpage, and peeling issues due to high silicone content, which affects the thinning process and heat treatment, while lacking adequate heat resistance and adhesive properties for laminating substrates.

Method used

A resin composition containing specific structural units, such as acid dianhydride and diamine residues, and a silane coupling agent, with controlled Si atom content and solvent viscosity, which provides improved adhesiveness, dimensional stability, and heat resistance, enabling uniform bonding and thin film formation without peeling or warping.

Benefits of technology

The resin composition ensures reliable adhesion and dimensional stability during heat treatment, preventing warpage and peeling, and maintaining heat resistance, thus enabling the production of ultra-thin semiconductor devices with enhanced reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011922_03102024_PF_FP_ABST
    Figure JP2024011922_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention pertains to a resin composition containing a solvent and a resin (A) having a structural unit represented by formula (1) and / or a structural unit represented by formula (2). With respect to a total of 100 mol% of acid dianhydride residues (X1) and (X2) and diamine residues (Y1) and (Y2) contained in the resin (A), the resin (A) contains a total of 10-40 mol% of at least one of an acid dianhydride residue (A1) having a structure represented by formula (3) and a diamine residue (A2) having a structure represented by formula (4). The resin (A) contains 1.0-20 mol% of a diamine residue (A3) having a structure represented by formula (5). The proportion of all Si atoms included in the resin (A) is 0.5-5.0 parts by mass with respect to 100 parts by mass of the resin (A). (Formulae (1)-(5) are as defined in the description.)
Need to check novelty before this filing date? Find Prior Art

Description

Resin composition, cured product, laminate, semiconductor device, and method for manufacturing semiconductor device

[0001] The present invention relates to a resin composition, a cured product, a laminate, a semiconductor device, and a method for manufacturing a semiconductor device. More specifically, the present invention relates to a resin composition suitable for thinning semiconductor devices, and a cured product, a laminate, a semiconductor device, and a method for manufacturing a semiconductor device using the same.

[0002] In recent years, semiconductor devices have been rapidly becoming smaller and thinner. For example, thinner devices are required to improve the processing speed and reduce costs of semiconductor devices. Display devices using μLEDs have also been proposed, and there is a demand for further miniaturization and thinning in order to improve the resolution of display devices and reduce the cost of μLED chips. When used for lighting, for example, further thinning is required in terms of design and cost reduction. Furthermore, these semiconductor devices are typically manufactured through heat treatment processes such as solder reflow and mechanical processes such as thinning. Therefore, adhesives used in these devices and components must not only be thin, but also be free of peeling or voids during and after the heat treatment and mechanical processes of the devices.

[0003] As adhesives for use in these semiconductor devices, etc., a technology has been proposed in which the glass transition temperature of a polyimide resin is designed to be 40°C or lower to improve adhesion (Patent Document 1), and a technology in which a crosslinkable group is introduced into a silicone-modified polyimide resin to impart heat resistance (Patent Document 2).Furthermore, a technology has been proposed in which the glass transition temperature of a polyimide resin is designed to be 300°C or higher to improve heat resistance and dimensional stability (Patent Document 3).

[0004] International Publication No. 2014 / 050878 Japanese Patent Application Publication No. 2019-172894 Japanese Patent Application Publication No. 2014-61685

[0005] The resin compositions of the inventions described in Patent Documents 1 and 2 contain a high content of silicone components, enabling devices to be bonded at low temperatures. However, due to the high content of flexible silicone components, they suffer from poor dimensional stability. This can lead to warping when bonding a device substrate to a support substrate, or twisting of the adhesive layer during ultra-thinning of the device, resulting in uneven thinning and damage to the device. Furthermore, heat treatment after device bonding can cause dimensional changes in the adhesive, resulting in device misalignment. The invention described in Patent Document 3 does not contain a component that imparts adhesiveness, making it inapplicable to semiconductor devices that use a method of laminating substrates together. Furthermore, the inventions described in Patent Documents 1 to 3 all require a thick adhesive layer because thinning the adhesive layer increases the risk of peeling, resulting in the adhesive layer's thickness affecting the device's thickness. Therefore, the present invention has been developed to solve the problems of the prior art and enable ultra-thinning of devices.

[0006] In order to solve the above problems, the present invention has the following configuration: [1] A resin composition containing a resin (A) having at least one structural unit selected from the structural units represented by formula (1) and the structural units represented by formula (2), and a solvent, wherein, relative to a total of 100 mol % of the acid dianhydride residues (X1) and (X2) and the diamine residues (Y1) and (Y2) contained in the resin (A), the resin (A) contains a total of 10 mol % to 40 mol % of at least one of the acid dianhydride residue (A1) having a structure represented by formula (3) and the diamine residue (A2) having a structure represented by formula (4), the resin (A) contains 1.0 mol % to 20 mol % of the diamine residue (A3) having a structure represented by formula (5), and the proportion of all Si atoms contained in the resin (A) is 0.5 parts by mass to 5.0 parts by mass per 100 parts by mass of the resin (A).

[0007]

[0008] (In formula (1) and formula (2), X 1 and X 2each independently represents a tetravalent acid dianhydride residue having 4 to 50 carbon atoms, and Y 1 and Y 2 R each independently represents a divalent diamine residue having 2 to 100 carbon atoms. 1 and R 2 each independently represents a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, an alkylsilyl group having 1 to 10 carbon atoms, an alkali metal atom, an ammonium group, an imidazolium group, or a pyridinium group.

[0009]

[0010] (In formulas (3) to (5), R 3 ~R 16 R each independently represents a hydrogen atom, a monovalent organic group having 1 to 20 carbon atoms, a hydroxyl group, or a halogen atom. 17 ~R 20 R each independently represents an alkyl group having 1 to 30 carbon atoms, an alkoxy group having 1 to 30 carbon atoms, a phenyl group, or a phenoxy group. 21 and R 22 each independently represents an alkylene group or a phenylene group having 1 to 30 carbon atoms, and n represents an integer of 1 to 20. * 3a and * 3b represents a bonding site connected to an imide group in the structural unit represented by formula (1), or * 3a represents a bonding site connected to the carbon atom of the amide bond in the structural unit represented by formula (2), * 3b represents a bonding site connecting to the carbon atom of the carboxylic acid or carboxylic acid ester in the structural unit represented by the formula (2). * 4, and * 5 represents a bonding site connecting to the nitrogen atom of the imide group in the structural unit represented by formula (1) or the amide bond in the structural unit represented by formula (2).

[0011] [2] The resin composition according to the above [1], wherein the diamine residue (A2) is a diamine residue having a structure represented by formula (6):

[0012]

[0013] (In formula (6), * 6 represents a bonding site connected to the nitrogen atom of the imide group in the structural unit represented by formula (1) or the amide bond in the structural unit represented by formula (2).

[0014] [3] The resin composition according to the above [1], wherein in the diamine residue (A3), n in the formula (5) is 1.

[0015] [4] The resin composition according to the above [1], wherein the solvent contained in the resin composition has a viscosity of 1.8 mPa·s or more and 3.1 mPa·s or less.

[0016] [5] The resin composition according to the above [1] or [2], further comprising a silane coupling agent.

[0017] [6] The resin composition according to the above [5], wherein the silane coupling agent contains a compound represented by formula (7):

[0018]

[0019] (In formula (7), R 23 represents an alkylene group having 5 to 10 carbon atoms. 24 each independently represents an alkyl group having 1 to 5 carbon atoms; and Z represents a hydrogen atom or a group represented by any one of the following formulas (8) to (14):

[0020]

[0021] (In formulas (8) to (14), R 25 ~R 31 each independently represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, a hydroxyl group, or a halogen atom. * 8~ * 14 is R in formula (7) 23 represents the binding site with

[0022] [7] The resin composition according to [1] or [2] above, further containing inorganic particles. [8] A cured product obtained by curing the resin composition of any one of [1] to [4] above. [9] A laminate having the cured product according to [8] above.

[10] The laminate according to [9] above, wherein the thickness of the cured product is 0.5 μm or more and 8.0 μm or less.

[11] The laminate according to

[10] above, wherein the laminate has a plurality of layers made of the cured product.

[12] The laminate according to

[10] above, wherein the laminate has a compound semiconductor layer.

[13] A semiconductor device having the laminate according to

[10] above.

[14] A method for manufacturing a semiconductor device, comprising at least one of a step of thinning the laminate according to

[10] above and a step of singulating the laminate according to

[10] above.

[0023] The resin composition of one embodiment of the present invention has excellent adhesiveness and can stably bond devices even when thin. Furthermore, the resin composition of one embodiment of the present invention has a low linear expansion coefficient, so warping is small when substrates are bonded together, and even when heat treatment is performed after bonding, the resin composition has excellent dimensional stability, reducing misalignment and peeling of bonded devices. Therefore, a semiconductor device including a cured product of the resin composition of one embodiment of the present invention has excellent reliability even when the cured product is thinly laminated.

[0024] FIG. 1 is an enlarged cross-sectional view of the mounting portion of an LED element of a monolithic LED. FIG. 2 is an enlarged view of a monolithic LED element 1. FIG. 3A shows an example of step (3-a) in the manufacturing process of a monolithic LED display. FIG. 3B shows an example of step (3-b) in the manufacturing process of a monolithic LED display. FIG. 3C shows an example of step (3-c) in the manufacturing process of a monolithic LED display. FIG. 3D shows an example of step (3-d) in the manufacturing process of a monolithic LED display. FIG. 3E shows an example of step (3-e) in the manufacturing process of a monolithic LED display. FIG. 3F shows an example of step (3-f) in the manufacturing process of a monolithic LED display. FIG. 3G shows an example of step (3-g) in the manufacturing process of a monolithic LED display. FIG. 3H shows an example of step (3-h) in the manufacturing process of a monolithic LED display. FIG. 3I shows an example of step (3-i) in the manufacturing process of a monolithic LED display. Figure 3J shows an example of step (3-j) in the manufacturing process of a monolithic LED display, and Figure 3K shows an example of step (3-k) in the manufacturing process of a monolithic LED display.

[0025] [Resin Composition] A resin composition according to one aspect of the present invention (hereinafter also referred to as "this embodiment") is a resin composition containing a resin (A) having at least one structural unit selected from the structural units represented by formula (1) and the structural units represented by formula (2), and a solvent, wherein, relative to a total of 100 mol % of the acid dianhydride residues (X1) and (X2) and the diamine residues (Y1) and (Y2) contained in the resin (A), the resin (A) contains a total of 10 mol % to 40 mol % of at least one of the acid dianhydride residue (A1) having a structure represented by formula (3) and the diamine residue (A2) having a structure represented by formula (4), the resin (A) contains 1.0 mol % to 20 mol % of the diamine residue (A3) having a structure represented by formula (5), and the proportion of all Si atoms contained in the resin (A) is 0.5 parts by mass to 5.0 parts by mass per 100 parts by mass of the resin (A).

[0026]

[0027] In formula (1) and formula (2), X 1 and X 2 each independently represents a tetravalent acid dianhydride residue having 4 to 50 carbon atoms, and Y 1 and Y 2 R each independently represents a divalent diamine residue having 2 to 100 carbon atoms. 1 and R 2 each independently represents a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, an alkylsilyl group having 1 to 10 carbon atoms, an alkali metal atom, an ammonium group, an imidazolium group, or a pyridinium group.

[0028]

[0029] In formulas (3) to (5), R 3 ~R 16 R each independently represents a hydrogen atom, a monovalent organic group having 1 to 20 carbon atoms, a hydroxyl group, or a halogen atom. 17 ~R 20 R each independently represents an alkyl group having 1 to 30 carbon atoms, an alkoxy group having 1 to 30 carbon atoms, a phenyl group, or a phenoxy group. 21 and R 22 each independently represents an alkylene group or a phenylene group having 1 to 30 carbon atoms, and n represents an integer of 1 to 20. * 3a and * 3b represents a bonding site connected to an imide group in the structural unit represented by the above formula (1), or * 3a represents a bonding site connected to the carbon atom of the amide bond in the structural unit represented by formula (2), * 3b represents a bonding site connected to the carbon atom of the carboxylic acid or carboxylic acid ester in the structural unit represented by the above formula (2). * 4, and * 5 represents a bonding site connected to the nitrogen atom of the imide group in the structural unit represented by formula (1) or the amide bond in the structural unit represented by formula (2).

[0030] (Resin (A)) The acid dianhydride residue (A1) having a structure represented by formula (3) (hereinafter also referred to as "acid dianhydride residue (A1)") and the diamine residue (A2) having a structure represented by formula (4) (hereinafter also referred to as "diamine residue (A2)") are residues of monomers having a biphenyl skeleton, and by containing at least one of them, a rigid structure can be introduced into the resin (A). The resin (A) contained in the resin composition contains at least one of the acid dianhydride residue (A1) and the diamine residue (A2) in a total amount of 10 mol % to 40 mol % relative to the total of the acid dianhydride residues (X1) and (X2) and the diamine residues (Y1) and (Y2) contained in the resin (A), 100 mol %.

[0031] The resin (A) contained in the resin composition contains at least one of the acid dianhydride residue (A1) and the diamine residue (A2) in a total amount of 10 mol% or more relative to the total 100 mol% of the acid dianhydride residues (X1) and (X2) and the diamine residues (Y1) and (Y2) contained in the resin (A). When the resin composition is cured by heat treatment, the cured product has a low linear expansion coefficient and is resistant to thermal deformation. This prevents warping of the device substrate and twisting of the film, which can damage the device substrate, when bonding substrates and devices together or when bonding and thinning device substrates. A more preferred range for the total amount of the acid dianhydride residue (A1) and the diamine residue (A2) is 15 mol% or more relative to the total 100 mol% of the acid dianhydride residues (X1) and (X2) and the diamine residues (Y1) and (Y2) contained in the resin (A). This further reduces the linear expansion coefficient of the formed cured film, and makes it possible to suppress warping of the laminate even in a configuration in which a plurality of cured products are stacked.

[0032] Furthermore, when the resin (A) contained in the resin composition contains at least one of the acid dianhydride residue (A1) and the diamine residue (A2) in a total amount of 40 mol% or less, relative to the total of 100 mol% of the acid dianhydride residues (X1) and (X2) and the diamine residues (Y1) and (Y2) contained in the resin (A), the glass transition temperature of the cured product obtained by curing the resin composition can be adjusted to an appropriate range. This allows substrates to be thermally laminated at temperatures that do not affect the device. A more preferred range for the total amount of the acid dianhydride residue (A1) and the diamine residue (A2) is 30 mol% or less, relative to 100 mol% of all monomer residues in the resin (A). This enables uniform lamination.

[0033] The acid dianhydride constituting the acid dianhydride residue (A1) may contain residues of known acid dianhydrides. Specific examples include 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,2'dimethyl-3,3',4,4'-biphenyltetracarboxylic dianhydride, and 5,5'dimethyl-3,3',4,4'-biphenyltetracarboxylic dianhydride. Among these, 3,3',4,4'-biphenyltetracarboxylic dianhydride is particularly preferred from the viewpoint of availability.

[0034] Examples of diamines constituting the diamine residue (A2) include 4,4'-biphenyldiamine, 2,2'-dimethylbiphenyl-4,4'-diamine, 4,4'-diamino-3,3',5,5'-tetramethylbiphenyl, 4,4'-diamino-3,3'-dimethylbiphenyl, 2,2'-benzidinedisulfonic acid, 4,4'-diamino-2,2'-bis(trifluoromethyl)biphenyl, 4,4'-diamino-3,3'-diethylbiphenyl dihydrochloride, octafluorobenzidine, and 4,4'-diamino-3,3'-dimethoxybiphenyl. Since this allows the resin (A) to have a more rigid structure, those having hydrogen or a methyl group as a substituent, such as 4,4'-biphenyldiamine, 2,2'-dimethylbiphenyl-4,4'-diamine, 4,4'-diamino-3,3',5,5'-tetramethylbiphenyl, and 4,4'-diamino-3,3'-dimethylbiphenyl, are preferred.

[0035] Among these, it is particularly preferred that the diamine residue (A2) be a diamine residue having a structure represented by the following formula (6): The effect of the methyl group is such that the solubility in solvents of the resin (A) can be improved while maintaining the rigidity of the resin (A). This allows for the production of a smooth coating film, and further suppresses poor lamination due to poor in-plane uniformity of the coating film during the substrate lamination step.

[0036]

[0037] In formula (6), * 6 represents a bonding site connected to the nitrogen atom of the imide group in the structural unit represented by the above formula (1) or the amide bond in the structural unit represented by the above formula (2).

[0038] An example of the diamine constituting the diamine residue having the structure represented by formula (6) is 2,2'-dimethylbiphenyl-4,4'-diamine.

[0039] The diamine residue (A3) having the structure represented by formula (5) (hereinafter also referred to as "diamine residue (A3)") is a flexible diamine residue having a siloxane bond.

[0040]

[0041] In formula (5), R 17 ~R 20 R each independently represents an alkyl group having 1 to 30 carbon atoms, an alkoxy group having 1 to 30 carbon atoms, a phenyl group, or a phenoxy group. 21 and R 22 may be the same or different and represent an alkylene group or a phenylene group having 1 to 30 carbon atoms. n is an integer of 1 to 20. When n is 1 or greater, the diamine residue (A3) has a silicone structure, and the resin composition can achieve high adhesiveness. Furthermore, when n is 20 or less, compatibility with other monomers is improved during polymerization of the resin (A), facilitating polymerization of the resin. A more preferred range for n is 10 or less, which allows the silicone structure-containing moieties to be dispersed in the resin (A), thereby achieving uniform adhesiveness in the coating film.

[0042] In the diamine residue (A3), the repeating unit n in formula (5) is preferably 1. When n = 1, adhesiveness can be imparted without impairing the rigidity of the film, thereby significantly improving dimensional stability, which is difficult to impart to conventional adhesives.

[0043] The resin (A) contained in the resin composition contains the diamine residue (A3) in an amount of 1.0 mol % or more and 20 mol % or less, relative to 100 mol % in total of the acid dianhydride residues (X1) and (X2) and the diamine residues (Y1) and (Y2) contained in the resin (A).

[0044] When the resin (A) contained in the resin composition contains 1.0 mol% or more of the diamine residue (A3) relative to the total 100 mol% of the acid dianhydride residues (X1) and (X2) and the diamine residues (Y1) and (Y2) contained in the resin (A), adhesiveness can be imparted to the resin composition (A). A more preferred content range of the diamine residue (A3) is 2.0 mol% or more relative to the total 100 mol% of the acid dianhydride residues (X1) and (X2) and the diamine residues (Y1) and (Y2) contained in the resin (A). This allows the diamine residue (A3), a component involved in adhesion, to be uniformly present in the resin (A). Therefore, uneven adhesion is less likely to occur during the substrate bonding process, and adhesion defects can be reduced, particularly when the resin composition is bonded in thin films.

[0045] In the resin (A) contained in the resin composition, the diamine residue (A3) is contained in an amount of 20 mol% or less, relative to the total 100 mol% of the acid dianhydride residues (X1) and (X2) and the diamine residues (Y1) and (Y2) contained in the resin (A). This improves heat resistance when the substrates are heated after bonding, thereby suppressing clouding and peeling of the film caused by decomposition gases. A more preferred range of the diamine residue (A3) is 17 mol% or less, relative to the total 100 mol% of the acid dianhydride residues (X1) and (X2) and the diamine residues (Y1) and (Y2) contained in the resin (A). This prevents excessive softening of the adhesive layer during heat treatment, and provides excellent dimensional stability during heat treatment.

[0046] As diamines constituting the diamine residue (A3), diamines where n=1 include tetramethyl-1,3-bis(3-aminopropyl)disiloxane, and diamines where n=2 or more include α,ω-bis(3-aminopropyl)polydimethylsiloxane, α,ω-bis(3-aminopropyl)polydiethylsiloxane, α,ω-bis(3-aminopropyl)polydipropylsiloxane, α,ω-bis(3-aminopropyl)polydibutylsiloxane, α,ω-bis(3-aminopropyl)polydiphenoxysiloxane, and α,ω-bis(2 Examples of suitable polydimethylsiloxanes include α,ω-bis(2-aminoethyl)polydimethylsiloxane, α,ω-bis(4-aminobutyl)polydimethylsiloxane, α,ω-bis(4-aminobutyl)polydiphenoxysiloxane, α,ω-bis(5-aminopentyl)polydimethylsiloxane, α,ω-bis(5-aminopentyl)polydiphenoxysiloxane, α,ω-bis(4-aminophenyl)polydimethylsiloxane, and α,ω-bis(4-aminophenyl)polydiphenoxysiloxane. n may be a single value or may be a mixture of multiple values ​​of n, so n in formula (5) represents an average value. From the viewpoints of availability and the ability to efficiently impart adhesiveness to the resin (A) without impairing its rigidity, the diamine constituting the diamine residue (A3) is preferably tetramethyl-1,3-bis(3-aminopropyl)disiloxane, α,ω-bis(3-aminopropyl)polydimethylsiloxane, or a combination thereof.

[0047] Preferred combinations of the acid dianhydride constituting the acid dianhydride residue (A1), the diamine constituting the diamine residue (A2), and the diamine constituting the diamine residue (A3) include a combination of 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,2'-dimethylbiphenyl-4,4'-diamine, and tetramethyl-1,3-bis(3-aminopropyl)disiloxane, and a combination of 3,3',4,4'-biphenyltetracarboxylic dianhydride, 4,4'-diamino-3,3'-dimethylbiphenyl, and α,ω-bis(3-aminopropyl)polydimethylsiloxane.

[0048] Resin (A) contains Si atoms in an amount of 0.5 parts by mass or more and 5.0 parts by mass or less per 100 parts by mass of resin (A). When resin (A) contains 0.5 parts by mass or more of Si atoms, it becomes possible to bond the entire surface of the substrate and the device substrate. A more preferable content of Si atoms is 2.0 parts by mass or more per 100 parts by mass of resin (A). When resin (A) contains Si atoms in this range, the adhesiveness is further improved, thereby preventing thin film substrate bonding and peeling after device singulation. Furthermore, when resin (A) contains 5.0 parts by mass or less of Si atoms per 100 parts by mass of resin (A), the heat resistance of resin (A) can be maintained high, thereby reducing substrate peeling and the occurrence of voids due to degassing when the bonded substrate is heat treated. A more preferable range of the Si atom content is 4.0 parts by mass or less per 100 parts by mass of resin (A). This allows both adhesiveness and dimensional stability to be achieved, allowing substrates to be bonded together without peeling or warping. The proportion of Si atoms in resin (A) can be determined by elemental analysis of resin (A).

[0049] Examples of the Si atom contained in the resin (A) include those derived from the diamine residue (A3) and those derived from a monomer having a silsesquioxane structure. When the resin (A) contains the diamine residue (A3), uniform adhesiveness can be imparted to the resin composition.

[0050] Furthermore, the resin (A) may have a monomer residue other than the acid dianhydride residue (A1), the diamine residue (A2), and the diamine residue (A3). Examples of such a monomer residue include residues of monomers having a silsesquioxane structure.

[0051] The acid dianhydride residue other than the acid dianhydride residue (A1) may contain residues of known acid dianhydrides, and preferably contains residues of aromatic tetracarboxylic acid dianhydrides. Specific examples of the residue of aromatic tetracarboxylic dianhydride include pyromellitic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-diphenylethertetracarboxylic dianhydride, 2,3,3',4'-diphenylethertetracarboxylic dianhydride, 2,2',3,3'-diphenylethertetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 2,2',3,3'-benzophenonetetracarboxylic dianhydride, 2,3,3',4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 2,3,3',4'-diphenylsulfonetetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfoxidetetracarboxylic dianhydride, 3,3',4 ,4'-diphenylsulfidetetracarboxylic dianhydride, 3,3',4,4'-diphenylmethylenetetracarboxylic dianhydride, 4,4'-isopropylidenediphthalic dianhydride, 4,4'-(hexafluoroisopropylidene)diphthalic dianhydride, 3,4,9,10-perylenetetracarboxylic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 1 , 2,5,6-naphthalenetetracarboxylic dianhydride, 3,3",4,4"-para-terphenyltetracarboxylic dianhydride, 3,3",4,4"-meta-terphenyltetracarboxylic dianhydride, 2,3,6,7-anthracenetetracarboxylic dianhydride, 1,2,7,8-phenanthrenetetracarboxylic dianhydride, 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride, and the like. The aromatic tetracarboxylic dianhydride residues may be one type or two or more types.

[0052] Resin (A) may contain a residue of a tetracarboxylic acid dianhydride having an aliphatic ring as an acid dianhydride residue other than the acid dianhydride residue (A1), to the extent that the heat resistance of resin (A) is not impaired. Specific examples of the residue of a tetracarboxylic acid dianhydride having an aliphatic ring include 2,3,5-tricarboxycyclopentylacetic acid dianhydride, 1,2,3,4-cyclobutane tetracarboxylic acid dianhydride, 1,2,3,4-cyclopentane tetracarboxylic acid dianhydride, 1,2,3,5-cyclopentane tetracarboxylic acid dianhydride, 1,2,4,5-bicyclohexene tetracarboxylic acid dianhydride, 1,2,4,5-cyclohexane tetracarboxylic acid dianhydride, 1,3,3a,4,5,9b-hexahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)-naphtho[1,2-C]furan-1,3-dione, and double-decker silsesquioxane alicyclic acid dianhydride. The resin (A) may contain only one type of residue of the tetracarboxylic dianhydride, or may contain two or more types.

[0053] Furthermore, the resin (A) may contain a residue of a known diamine as a diamine residue other than the diamine residue (A2) and the diamine residue (A3). Specific examples of the diamine include p-phenylenediamine, m-phenylenediamine, 2,5-diaminotoluene, 2,4-diaminotoluene, 3,5-diaminobenzoic acid, 2,6-diaminobenzoic acid, 2-methoxy-1,4-phenylenediamine, 4,4'-diaminobenzanilide, 3,4'-diaminobenzanilide, 3,3'-diaminobenzanilide, 3,3'-dimethyl-4,4'-diaminobenzanilide, 9,9-bis(4-aminophenyl)fluorene, and 9,9-bis(3-aminophenyl)fluorene. fluorene, 9,9-bis(3-methyl-4-aminophenyl)fluorene, 9,9-bis(3,5-dimethyl-4-aminophenyl)fluorene, 9,9-bis(3-methoxy-4-aminophenyl)fluorene, 9,9-bis(4-aminophenyl)fluorene-4-carboxylic acid, 9,9-bis(4-aminophenyl)fluorene-4-methyl, 9,9-bis(4-aminophenyl)fluorene-4-methoxy, 9,9-bis(4-aminophenyl)fluorene-4-ethyl, 9,9-bis(4-aminophenyl)fluorene 9,9-bis(4-aminophenyl)fluorene-4-sulfone, 9,9-bis(4-aminophenyl)fluorene-3-carboxylic acid, 9,9-bis(4-aminophenyl)fluorene-3-methyl, 1,3-diaminocyclohexane, 2,2'-dimethylbenzidine, 3,3'-dimethylbenzidine, 3,3'-dimethoxybenzidine, 2,4-diaminopyridine, 2,6-diaminopyridine, 1,5-diaminonaphthalene, 2,7-diaminofluorene, p-aminobenzylamine, m-aminobenzylamine, 4,4' ... (aminophenoxy)biphenyl, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 3,3'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl sulfide, 3,3'-diaminobenzophenone, 3,4'-diaminobenzophenone, 4,4'-diaminobenzophenone, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 1,3-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 1,4-bis(3-aminophenoxy)benzene, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(3-aminophenoxy)phenyl]propane, bis[4-(4-aminophenoxy)phenyl]methane, bis[4-(3-aminophenoxy)phenyl]methane, bis[4-(4-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl] phenyl] ether, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 1,4-diaminocyclohexane, 4,4'-methylenebis(cyclohexylamine), 3,3'-methylenebis(cyclohexylamine), 4,4'-diamino-3,3'-dimethyldicyclohexylmethane, 4,4'-diamino-3,3'-dimethyldicyclohexyl, 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, etc. Resin (A) may contain the above diamine residues alone or in combination of two or more.

[0054] The molecular weight of resin (A) can be adjusted by using equimolar amounts of the acid dianhydride component and the diamine component used in the synthesis, or by using an excess of either one. Either the acid dianhydride component or the diamine component can be used in excess, and the polymer chain ends can be capped with an end-capping agent such as an acid component or an amine component. Dicarboxylic acids or their anhydrides are preferably used as end-capping agents for the acid component, and monoamines are preferably used as end-capping agents for the amine component. In this case, it is preferable to use equimolar amounts of the acid equivalent of the tetracarboxylic acid component, including the end-capping agent for the acid component or the amine component, and the amine equivalent of the diamine component.

[0055] Known monoamines can be used as the terminal blocking agent for the amine component, and among them, preferred are aniline, 5-amino-8-hydroxyquinoline, 1-hydroxy-5-aminonaphthalene, 1-hydroxy-4-aminonaphthalene, 2-carboxy-6-aminonaphthalene, 3-amino-4,6-dihydroxypyrimidine, 3-aminophenol, 4-aminophenol, etc. Two or more of these may be used as the terminal blocking agent for the amine component.

[0056] Preferred examples of the acid component end-capping agent include monocarboxylic acids, monoacid chloride compounds, and monoactive ester compounds; acid anhydrides such as phthalic anhydride, maleic anhydride, nadic anhydride, and cyclohexanedicarboxylic anhydride; monocarboxylic acids such as 3-carboxyphenol and 1-hydroxy-6-carboxynaphthalene, and monoacid chloride compounds in which the carboxyl groups of these monocarboxylic acids are converted to acid chlorides; monoacid chloride compounds in which only one carboxyl group of dicarboxylic acids such as terephthalic acid, phthalic acid, and maleic acid is converted to acid chlorides; and active ester compounds obtained by reacting a monoacid chloride compound with N-hydroxybenzotriazole, imidazole, or N-hydroxy-5-norbornene-2,3-dicarboximide. Two or more of these acid component end-capping agents may be used.

[0057] The weight average molecular weight of resin (A) is preferably 5,000 or more and 50,000 or less. The weight average molecular weight of resin (A) is preferably 5,000 or more from the viewpoint of heat resistance, and more preferably 8,000 or more from the viewpoint of reliability when used permanently as an adhesive in a device. From the viewpoint of viscosity of the resin composition when handling film formation and varnish, it is preferably 50,000 or less, and from the viewpoint of ease of production of resin (A), it is more preferably 30,000 or less. Here, the weight average molecular weight of resin (A) can be calculated as a polystyrene equivalent value by performing gel permeation chromatography (GPC) analysis on a solution of resin (A) dissolved in N-methyl-2-pyrrolidone at a resin concentration of 0.1 wt %.

[0058] Furthermore, from the viewpoint of adhesiveness, the proportion of F atoms contained in the resin (A) is preferably low, and is preferably 2.0 parts by mass or less per 100 parts by mass of the resin (A). This allows for high adhesiveness to the substrate. More preferably, the content of F atoms is 0.2 parts by mass or less per 100 parts by mass of the resin (A). This allows for high adhesiveness when the resin layer is made thin.

[0059] The molar ratio of the acid dianhydride component to the diamine component of the resin (A) can be adjusted appropriately so that the resin composition containing the resin (A) is within a range that makes it easy to use in coating, etc. Typically, the molar ratio of the acid dianhydride component to the diamine component is adjusted within a range of 100 / 100 to 100 / 95, or 100 / 100 to 95 / 100. If the molar ratio of the acid dianhydride component to the diamine component of the resin (A) is outside the above range, the molecular weight of the resin (A) decreases, and the mechanical strength of the formed film decreases. This can result in uneven adhesive strength, so it is preferable to adjust the molar ratio within a range that stabilizes adhesive strength.

[0060] The resin (A) may be a polyimide precursor that undergoes ring closure upon heating to become a polyimide, a polyimide that has undergone ring closure upon heating, or a polyimide precursor in which a portion of the resin has undergone ring closure upon heating.

[0061] There are no particular limitations on the method for polymerizing resin (A). For example, when polymerizing polyamic acid, which is a polyimide precursor, tetracarboxylic dianhydride and diamine are stirred in an organic solvent at 0 to 100°C for 1 to 100 hours to obtain a polyamic acid resin solution. If resin (A) is soluble in an organic solvent, after polymerizing the polyamic acid, the temperature is raised to 120 to 300°C and the mixture is stirred for 1 to 100 hours to convert it to polyimide, thereby obtaining a solution of resin (A). At this time, toluene, o-xylene, m-xylene, p-xylene, or the like may be added to the reaction solution, and the water produced in the imidization reaction may be removed by azeotropy with the solvent.

[0062] (Solvent) The resin composition of this embodiment contains a solvent. By including a solvent, the viscosity of the resin composition can be adjusted, and the thickness of the cured product, which will be described later, can be adjusted. The content of the solvent is preferably 100 parts by mass or more and 2000 parts by mass or less per 100 parts by mass of the resin (A), and can be selected according to the desired film thickness. As the solvent used in the resin composition of this embodiment, the solvent used in the polymerization may be used as is, or a mixed solvent may be prepared by adding another solvent thereto. Alternatively, the polymerization solvent may be removed from the polymerization solution of the polymerized resin (A), and the resin (A) may be mixed with another solvent to prepare a resin composition. Specific examples of the solvent include polar aprotic solvents such as gamma butyrolactone, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono-n-propyl ether, ethylene glycol mono-n-butyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol mono-n-propyl ether, diethylene glycol mono-n-butyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, propylene glycol mono-n-butyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, ethers such as ethylene glycol monoethyl ether, dipropylene glycol mono-n-propyl ether, dipropylene glycol mono-n-butyl ether, tripropylene glycol monomethyl ether, tripropylene glycol monoethyl ether, tetrahydrofuran, and dioxane; ketones such as acetone, methyl ethyl ketone, diisobutyl ketone, cyclohexanone, cyclopentanone, 2-heptanone, 3-heptanone, and diacetone alcohol; ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, ethyl lactate,Ethyl 2-hydroxy-2-methylpropionate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, ethyl ethoxyacetate, ethyl hydroxyacetate, methyl 2-hydroxy-3-methylbutanoate, 3-methoxybutyl acetate, 3-methyl-3-methoxybutyl acetate, 3-methyl-3-methoxybutylpropionate, ethyl acetate, n-propyl acetate, i-propyl acetate, n-butyl acetate, i-acetate Examples of suitable solvents include esters such as n-butyl, n-pentyl formate, i-pentyl acetate, n-butyl propionate, ethyl butyrate, n-propyl butyrate, i-propyl butyrate, n-butyl butyrate, methyl pyruvate, ethyl pyruvate, n-propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, and ethyl 2-oxobutanoate; aromatic hydrocarbons such as toluene and xylene; and amides such as N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, and N-diethylacetamide. Of these, N-methylpyrrolidone, N-dimethylacetamide, N-diethylacetamide, cyclohexanone, and ethyl lactate are preferred. The solvents may be used alone or in combination, and are not limited to the above-mentioned solvents as long as they are compatible with the resin (A).

[0063] Furthermore, the viscosity of the solvent is preferably 1.8 mPa·s or more and 3.1 mPa·s or less. By using a solvent with a viscosity of 1.8 mPa·s or more, when applying the resin composition to a substrate, shrinkage of the coating film at the edge of the substrate and wraparound to the back surface of the substrate can be suppressed. The uniformity of the film thickness at the edge improves adhesion at the edge, and conveyance errors during processing can also be suppressed. Furthermore, by using a solvent with a viscosity of 3.1 mPa or less, the in-plane uniformity of the coating film can be improved. Examples of solvents with a viscosity of 1.8 mPa·s or more and 3.1 mPa·s or less include diacetone alcohol (viscosity: 2.90 mPa·s), cyclohexanone (viscosity: 1.97 mPa·s), ethyl lactate (2.44 mPa·s), dimethylimidazolidinone (viscosity: 2.63 mPa·s), and 3-methoxy-N,N-dimethylpropanamide (viscosity: 2.04 mPa·s).

[0064] (Silane Coupling Agent) The resin composition of this embodiment preferably contains a silane coupling agent. The silane coupling agent is preferably added at room temperature to 50°C after polymerizing the resin (A). By containing the silane coupling agent in the resin composition, the adhesion of the resin composition to a substrate can be improved. The content of the silane coupling agent in the resin composition is preferably 1.0 part by mass or more and 10 parts by mass or less per 100 parts by mass of the resin (A). By containing 1.0 part by mass or more of the silane coupling agent in the resin composition, the effect of improving the adhesion to the substrate can be obtained. It is more preferable that the resin composition contains 3.0 parts by mass or more of the silane coupling agent per 100 parts by mass of the resin (A). This makes it possible to suppress peeling of the device substrate or the singulated substrate, even when the device is subjected to a thinning or singulation process after bonding the substrates. Furthermore, by containing 10 parts by mass or less of the silane coupling agent in the resin composition per 100 parts by mass of the resin (A), it is possible to suppress degassing caused by the silane coupling agent during heat treatment. A more preferred content of the silane coupling agent in the resin composition is 7.0 parts by mass or less per 100 parts by mass of the resin (A). By including the silane coupling agent in this range, the storage stability of the varnish is improved. Examples of silane coupling agents include vinyltrimethoxysilane, vinyltriethoxysilane, epoxycyclohexylethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, p-styryltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, 7-octenyltrimethoxysilane, 8-glycidoxyoctyltrimethoxysilane, 8-methacryloxyoctyltrimethoxysilane, and N-2-(aminoethyl)-8-aminooctyltrimethoxysilane. These silane coupling agents may be used alone or in combination of two or more. The silane coupling agent more preferably contains a compound represented by formula (7).

[0065]

[0066] In formula (7), R 23 represents an alkylene group having 5 to 10 carbon atoms. 24 each independently represents an alkyl group having 1 to 5 carbon atoms. Z represents a hydrogen atom or a group represented by any one of the following formulas (8) to (14).

[0067]

[0068] In formulas (8) to (14), R 25 ~R 31 each independently represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, a hydroxyl group, or a halogen atom. * 8~ * 14 is R in formula (7) 23 represents the binding site with

[0069] Examples of silane coupling agents having a structure represented by formula (8) include 8-glycidoxyoctyltrimethoxysilane and 6-glycidoxyhexyltrimethoxysilane. Examples of silane coupling agents having a structure represented by formula (9) include 7-octenyltrimethoxysilane and 7-octenyltriethoxysilane. Examples of silane coupling agents having a structure represented by formula (10) include 8-methacryloxyoctyltrimethoxysilane. Examples of silane coupling agents having a structure represented by formula (11) include N-2-(aminoethyl)-8-aminooctyltrimethoxysilane and N-2-(aminoethyl)-6-aminohexyltrimethoxysilane. Examples of silane coupling agents having a structure represented by formula (12) include 1-(6-(trimethoxysilyl)hexyl)urea). Examples of silane coupling agents having a structure represented by formula (13) include 1-(6-(trimethoxysilyl)hexyl)thiourea). Examples of silane coupling agents having the structure represented by formula (14) include 8-phenyloctyltrimethoxysilane.

[0070] The silane coupling agent containing the compound represented by formula (7) has good compatibility with the resin (A) and has a higher effect of improving adhesion, so that peeling can be prevented even when the substrates after bonding are subjected to a heat treatment of 250° C. or more. The preferred amount of the silane coupling agent containing the compound represented by formula (7) to be added is the same as the preferred amount of the silane coupling agent described above.

[0071] (Inorganic Particles) The resin composition of this embodiment may contain inorganic particles from the viewpoint of improving dimensional stability and heat resistance. The content of the inorganic particles in the resin composition is preferably 2.0 parts by mass or more and 10 parts by mass or less per 100 parts by mass of resin (A). When the content of the inorganic particles in the resin composition is 2.0 parts by mass or more per 100 parts by mass of resin (A), the effect of improving dimensional stability is obtained. When the content of the inorganic particles in the resin composition is 10 parts by mass or less per 100 parts by mass of resin (A), the adhesiveness of the resin composition is maintained. Examples of inorganic particles include silica, alumina, titanium oxide, quartz powder, magnesium carbonate, potassium carbonate, barium sulfate, mica, and talc. In particular, silica particles are preferred from the viewpoint of heat resistance.

[0072] (Crosslinking Agent) The resin composition of the present embodiment may contain a crosslinking agent. By containing a crosslinking agent, the chemical resistance and heat resistance of the resin composition are improved after curing, and the processability and reliability of the device are improved. As the crosslinking agent, a known crosslinking agent can be used, and an epoxy-based crosslinking agent, an acrylic-based crosslinking agent, a methylol-based crosslinking agent, or the like can be selected.

[0073] (Resins Other Than Resin (A)) The resin composition of this embodiment may contain resins other than resin (A) as long as the effects of the present invention are not impaired. Furthermore, surfactants may be added for the purpose of improving properties such as adhesion, heat resistance, coatability, and storage stability. Furthermore, other resins and surfactants may be added during or after polymerization of resin (A).

[0074] Other resins include acrylic resins, epoxy resins, polystyrene resins, novolac resins, polybenzoxazole resins, and silicone resins. Surfactants include silane-based surfactants, acrylic surfactants, and fluorine-based surfactants. [Cured Product] Next, the cured product of this embodiment will be described. A cured product of the resin composition is obtained by curing the resin composition, and the resin composition is preferably cured by heat treatment. When resin (A) is a polyamic acid resin, it can be converted to polyimide by heat treatment. Heat treatment can be performed using an oven, a hot plate, infrared rays, or the like. The curing temperature and curing time are the temperature and time required to volatilize the solvent contained in the resin composition and convert resin (A) into a film that does not flow at room temperature. Specifically, the curing temperature is 100°C to 300°C, and the curing time is several minutes to several hours.

[0075] The cured product may be a film-like cured product prepared by forming a coating film from the resin composition. By forming the cured product into a film, the thickness of the cured product can be made uniform, eliminating unevenness in the subsequent formation of a laminate or bonding to a device substrate. A method for forming the cured product into a film includes applying the resin composition to a substrate or the like, followed by the above-mentioned heat treatment. The resin composition can be applied by any known method, including spin coating using a spinner, spray coating, roll coating, screen printing, a blade coater, a die coater, a calendar coater, a meniscus coater, a bar coater, a roll coater, a comma roll coater, a gravure coater, a screen coater, and a slit die coater.

[0076] The glass transition temperature of the cured product is preferably 150°C or higher from the viewpoint of dimensional stability during heat treatment, and is preferably 260°C or lower from the viewpoint of ease of lamination. The glass transition temperature can be measured using a differential scanning calorimeter (DSC) or thermomechanical analysis (TMA). A more detailed method for measuring the glass transition temperature is as described in the Examples below.

[0077] The coefficient of linear thermal expansion (CTE) of the cured product is preferably 30 ppm / K or more from the viewpoint of adhesiveness, and is preferably 100 ppm / K or less from the viewpoint of reducing warping when bonding devices or substrates and peeling caused by warping. The coefficient of linear thermal expansion can be calculated, for example, according to the following formula (X) as the rate of change in sample length from a temperature 80°C lower to a temperature 30°C lower than the glass transition temperature of each cured product: CTE (1 / K) = ((sample length (m) at Tg - 30°C)) - (sample length (m) at Tg - 80°C) / (sample length (m) before measurement × 50 (K)) Formula (X)

[0078] The change in sample length due to temperature can be measured using thermomechanical analysis (TMA). A more detailed method for measuring the linear thermal expansion coefficient is as described in the Examples below.

[0079] The 1% weight loss temperature of the cured product is preferably 300°C or higher and 600°C or lower, from the viewpoint of heat resistance required in processes using the cured product. The 1% weight loss temperature is measured using a thermogravimetric analyzer. In this case, the temperature is determined by holding the product at 120°C for 30 minutes and then increasing the temperature to 500°C at a rate of 5°C / min.

[0080] [Laminate] Next, a laminate having the cured product will be described. The laminate of this embodiment is preferably one in which the cured product is laminated on a substrate. Specific examples of the substrate include inorganic substrates, organic substrates, and organic films such as films. More specific examples include substrates such as silicon, alkali glass, alkali-free glass, borosilicate glass, sapphire, quartz, and ceramic; substrates containing II-VI compound semiconductors such as ZnS and ZnCe; III-V compound semiconductors such as GaN, InP, GaAs, AlN, and GaAlAs; IV-IV compound semiconductors such as SiC; substrates containing oxide semiconductors such as LT, LN, and IGZO; and organic substrates and films such as PET, aramid, polyester, polypropylene, cycloolefin, and polyimide. These substrates also include combinations of these, as well as substrates on which circuits, patterns, and elements are formed. A method for forming a film-like cured product can be used to form a cured product on a substrate.

[0081] Since the cured product of this embodiment can be used as a temporary adhesive or a permanent adhesive, the laminate may be configured by bonding the above-mentioned substrates together with the cured product, or by bonding singulated elements to the above-mentioned laminate. The substrates bonded together with the cured product may be the same or different. Depending on the application, device substrates may be bonded together, or a device substrate may be bonded to a support substrate that protects it. A laminate in which substrates are bonded together can be produced by bonding another substrate to the exposed surface of the cured product of a laminate in which the cured product is laminated on the above-mentioned substrate. Examples of bonding methods include pressure bonding using a press, a roll laminator, etc., and when laminating singulated elements, a flip-chip bonder can also be used. When bonding, heating and compression bonding may be performed as necessary. The temperature at this time is preferably 50°C or higher and 250°C or lower, and a more preferred compression temperature is above the glass transition temperature of the resin (A). By setting the compression temperature at or above the glass transition temperature of the resin (A), the adhesiveness of the resin (A) is improved, allowing the substrates to be uniformly bonded to each other. The pressure bonding temperature is preferably 200°C or lower. This can suppress damage to the device substrate. The pressure during pressure bonding is preferably 0.1 MPa or higher and 5.0 MPa or lower, more preferably 0.2 MPa or higher and 3.0 MPa or lower. Pressure bonding may be performed in air or nitrogen. It is preferable to perform the pressure bonding under reduced pressure conditions or in a vacuum, as this can reduce air entrapment during pressure bonding.

[0082] Furthermore, the laminate may have a plurality of layers made of a cured product. A laminate having a plurality of layers made of a cured product can be produced by repeatedly forming a cured product on one surface of the laminate obtained by bonding the above-mentioned substrates together, or a laminate obtained by bonding a substrate and a singulated element, and then pressure-bonding the surface on which the cured product is exposed to another substrate or a singulated element. Alternatively, the laminate can be produced by repeatedly pressure-bonding one surface of a laminate obtained by bonding substrates together, or a laminate obtained by bonding a substrate and a singulated element, to the surface on which the cured product is exposed of a laminate obtained by separately forming a cured film on another substrate or a singulated element.

[0083] The thickness of the cured product in the laminate is preferably 0.5 μm or more and 8.0 μm or less. The thickness of the cured product in the laminate is preferably 0.5 μm or more, which enables stable bonding of the substrates. More preferably, the thickness of the cured product is 1.0 μm or more, which enables the device to be passed through the thinning heat treatment process after bonding without causing damage or peeling. Furthermore, the thickness of the cured product is preferably 8.0 μm or less, which reduces the effect of the adhesive thickness on thin devices. More preferably, it is 5.0 μm or less, which reduces warping of the laminate. The thickness of the cured film can be measured using a scanning electron microscope, an optical film thickness meter, a step gauge, a laser microscope, or the like.

[0084] The laminate preferably has a compound semiconductor layer, and such a laminate can be applied to various semiconductor devices such as high-frequency devices, high-power devices, laser diodes, and light-emitting diode-based lighting and displays. The compound semiconductor layer is a layer made of a compound semiconductor. Examples of compound semiconductors include, but are not limited to, those exemplified in the description of the laminate above.

[0085] [Semiconductor Device] This embodiment is a semiconductor device having the above-described laminate. As an application example using the laminate of this embodiment, a semiconductor device having a semiconductor element will be described with reference to the drawings, taking as an example a display using a monolithic LED element. Figure 1 is an enlarged cross-sectional view of the mounting portion of the LED element of a monolithic LED. Figure 1 shows a state in which a monolithic LED element 1 is mounted on a circuit board 2 so as to be electrically connected to the circuit board 2.

[0086] Next, FIG. 2 shows an enlarged view of the monolithic LED element 1. A first LED layer 10, which includes a first n-type GaN layer 111, a first light-emitting layer 112, a first p-type GaN layer 113, and a first transparent electrode 114 formed in this order on a first sapphire substrate 110, is laminated on a second LED layer 20, which includes a second n-type GaN layer 121, a second light-emitting layer 122, a second p-type GaN layer 123, and a second transparent electrode 124 formed in this order, via a second adhesive layer 220 made of the cured product of this embodiment at the interface between the first transparent electrode 114 and the second transparent electrode 124. ITO or the like can be used for the transparent electrode. The second LED layer is further laminated on a third LED layer 30, which includes a third n-type GaN layer 131, a third light-emitting layer 132, a third p-type GaN layer 133, and a third transparent electrode 134 formed in this order, via a third adhesive layer 230 made of the cured product of this embodiment at the interface between the second n-type GaN layer 121 and the third transparent electrode 134. Furthermore, each layer is electrically connected by electrodes 320, and portions other than the connected layers are insulated by passivation layers 310. The laminate using the cured product of this embodiment has excellent dimensional stability, so even when such a laminate having many layers is formed, it does not warp or peel, and a highly reliable device can be produced.

[0087] This embodiment is a method for manufacturing a semiconductor device using the laminate of this embodiment, and is characterized by including at least one of a step of thinning the laminate and a step of singulating the laminate. The method for manufacturing a semiconductor device may include a step of thinning the device.

[0088] As a method for manufacturing a semiconductor device, a method for manufacturing a monolithic LED element will be described with reference to the drawings. Figures 3A to 3K show an example of a manufacturing process for the monolithic LED display shown in Figure 1.

[0089] First, as shown in FIG. 3A , a first n-type GaN layer 111, a first light-emitting layer 112, and a first p-type GaN layer 113 are epitaxially grown in this order on a first sapphire substrate 110 using a known method. Furthermore, ITO is formed by vapor deposition on the surface of the first p-type GaN layer 113 as a first transparent electrode 114, and a stacked body is prepared in which a first LED layer 10 is stacked on the first sapphire substrate 110. Furthermore, an electrode via is formed from the first transparent electrode 114 side to the first n-type GaN layer 111. A known method can be used to form the via, and dry etching, for example, is applicable. This process is referred to as step (3-a).

[0090] Next, as shown in Figure 3B, a second LED layer 20 is formed on the second sapphire substrate 120 using the same method as described above, and a second adhesive layer 220 made of the cured product of this embodiment is formed on the surface of the second transparent electrode 124. Next, the surface of the first transparent electrode 114 of the first LED layer 10 and the surface of the second adhesive layer 220 are brought face to face, and the two laminates are bonded together. A known bonding device can be used for bonding, and it is particularly preferable to use a wafer bonder and perform the bonding while heating under reduced pressure conditions. This process is referred to as step (3-b).

[0091] Next, as shown in FIG. 3C, the second sapphire substrate 120 is removed. Removal methods include mechanical removal by polishing and laser removal, with laser removal being preferred in terms of processing speed and reuse of the sapphire substrate. When removing the sapphire substrate with a laser, a laser with a wavelength that penetrates the sapphire substrate is irradiated from the surface of the sapphire substrate opposite the surface that contacts the n-type GaN layer, and the n-type GaN layer is ablated at the interface between the sapphire substrate and the n-type GaN layer, thereby removing the sapphire substrate. Examples of laser wavelengths used to remove the sapphire substrate include 248 nm and 266 nm. This is step (3-c).

[0092] 3D, vias are formed from the side of second n-type GaN layer 121. The vias are formed so as to reach the via formed in step (3-a), first transparent electrode 114, and second transparent electrode 124. This is referred to as step (3-d).

[0093] 3E, a stacked body prepared in the same manner as in step (3-b), in which a third sapphire substrate 130, a third LED layer 30, and a third adhesive layer 230 made of the cured product of this embodiment are laminated in this order, is bonded to the surface of the second n-type GaN layer 121 of the stacked body prepared in step (3-d) at the surface of the third adhesive layer 230, thereby obtaining a stacked body in which the first LED layer 10 to the third LED layer 30 are laminated. This process is referred to as step (3-e).

[0094] 3F, the first sapphire substrate 110 of the laminate is thinned by polishing, and then the third sapphire substrate 130 is peeled off and removed. This is step (3-f).

[0095] 3G, vias are formed from the surface of third n-type GaN layer 131. The vias are formed so as to reach the already formed vias, second n-type GaN layer 121, and third transparent electrode 134. This is referred to as step (3-g).

[0096] Next, as shown in Fig. 3H, a passivation layer 310 is formed on the surface of the third n-type GaN layer 131 and on the side surfaces of each via. The passivation layer can be formed by a known method, and is typically made of SiO 2 These inorganic materials can be formed by sputtering using resist or a metal mask. This is the process (3-h).

[0097] As shown in Figure 3I, the inside of the via and the conductive portion with the circuit board 2 are filled with a metal to form an electrode using a plating method or the like, to create an electrode 320. The electrode material is preferably Au or an alloy thereof. This is step (3-i).

[0098] As shown in Figure 3J, the completed LED device is then singulated into individual pieces to the size of the element. The singulation is preferably performed using a mask, such as a dry etching method. This is referred to as step (3-j).

[0099] Finally, as shown in Figure 3K, the obtained LED element is mounted on circuit board 2. Known devices can be used for mounting, including a method of individually mounting LED elements at desired positions on a circuit board using a flip-chip bonder or the like, a method of mounting multiple LED elements at once using a stamp method, and a laser transfer method in which an LED element is temporarily bonded to the exposed surface of a laser-transparent substrate on which another transfer material has been laminated, and then a laser is irradiated from the laser-transparent substrate side to mount it at the desired position. This is step (3-k).

[0100] As described above, the present specification discloses the following: <1> A resin composition containing a resin (A) having at least one structural unit selected from the structural units represented by formula (1) and the structural units represented by formula (2), and a solvent, wherein, relative to a total of 100 mol % of the acid dianhydride residues (X1) and (X2) and the diamine residues (Y1) and (Y2) contained in the resin (A), the resin (A) contains a total of 10 mol % to 40 mol % of at least one of the acid dianhydride residue (A1) having a structure represented by formula (3) and the diamine residue (A2) having a structure represented by formula (4), the resin (A) contains 1.0 mol % to 20 mol % of the diamine residue (A3) having a structure represented by formula (5), and the proportion of all Si atoms contained in the resin (A) is 0.5 parts by mass to 5.0 parts by mass per 100 parts by mass of the resin (A).

[0101]

[0102] (In formula (1) and formula (2), X 1 and X 2 each independently represents a tetravalent acid dianhydride residue having 4 to 50 carbon atoms, and Y 1 and Y 2 R each independently represents a divalent diamine residue having 2 to 100 carbon atoms. 1 and R 2 each independently represents a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, an alkylsilyl group having 1 to 10 carbon atoms, an alkali metal atom, an ammonium group, an imidazolium group, or a pyridinium group.

[0103]

[0104] (In formulas (3) to (5), R 3 ~R 16 R each independently represents a hydrogen atom, a monovalent organic group having 1 to 20 carbon atoms, a hydroxyl group, or a halogen atom. 17 ~R 20 R each independently represents an alkyl group having 1 to 30 carbon atoms, an alkoxy group having 1 to 30 carbon atoms, a phenyl group, or a phenoxy group. 21 and R 22 each independently represents an alkylene group or a phenylene group having 1 to 30 carbon atoms, and n represents an integer of 1 to 20. * 3a and * 3b represents a bonding site connected to an imide group in the structural unit represented by formula (1), or * 3a represents a bonding site connected to the carbon atom of the amide bond in the structural unit represented by formula (2), * 3b represents a bonding site connecting to the carbon atom of the carboxylic acid or carboxylic acid ester in the structural unit represented by the formula (2). * 4, and * 5 represents a bonding site connecting to the nitrogen atom of the imide group in the structural unit represented by formula (1) or the amide bond in the structural unit represented by formula (2).

[0105] <2> The resin composition according to the above <1>, wherein the diamine residue (A2) is a diamine residue having a structure represented by formula (6):

[0106]

[0107] (In formula (6), * 6 represents a bonding site connected to the nitrogen atom of the imide group in the structural unit represented by formula (1) or the amide bond in the structural unit represented by formula (2).

[0108] <3> The resin composition according to <1> above, wherein in the diamine residue (A3), n in the formula (5) is 1.

[0109] <4> The resin composition according to <1> above, wherein the solvent contained in the resin composition has a viscosity of 1.8 mPa·s or more and 3.1 mPa·s or less.

[0110] <5> The resin composition according to <1> or <2> above, further comprising a silane coupling agent.

[0111] <6> The resin composition according to <5> above, wherein the silane coupling agent contains a compound represented by formula (7):

[0112]

[0113] (In formula (7), R 23 represents an alkylene group having 5 to 10 carbon atoms. 24 each independently represents an alkyl group having 1 to 5 carbon atoms; and Z represents a hydrogen atom or a group represented by any one of the following formulas (8) to (14):

[0114] (In formulas (8) to (14), R 25 ~R 31 each independently represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, a hydroxyl group, or a halogen atom. * 8~ * 14 is R in formula (7) 23 represents the binding site with

[0115] <7> The resin composition according to any one of <1> to <6> above, further comprising inorganic particles. <8> A cured product obtained by curing the resin composition according to any one of <1> to <7> above. <9> A laminate having the cured product according to <8> above. <10> The laminate according to <9> above, wherein the thickness of the cured product is 0.5 μm or more and 8.0 μm or less. <11> The laminate according to <9> or <10> above, wherein the laminate has a plurality of layers each composed of the cured product. <12> The laminate according to any one of <7> to <9> above, wherein the laminate has a compound semiconductor layer. <13> A semiconductor device having the laminate according to any one of <9> to <11> above. <14> A method for manufacturing a semiconductor device, comprising at least one of a step of thinning the laminate according to any one of <9> to <11> above and a step of singulating the laminate according to any one of <9> to <11> above.

[0116] The present invention will be described below with reference to examples, but the present invention is not limited to these examples.

[0117] <Evaluation Methods> (1) Measurement of Glass Transition Temperature and Linear Thermal Expansion Coefficient. Resin compositions 1 to 43 obtained in the following production examples were applied to the shiny surface of an 18 μm-thick electrolytic copper foil using a bar coater to a cured thickness of 10 μm. The resin was then dried at 80°C for 10 minutes and further heat-treated at 250°C for 30 minutes in a nitrogen atmosphere to cure the resin, yielding a resin-laminated copper foil. The copper foil of the resulting resin-laminated copper foil was then completely etched with a ferric chloride solution to obtain a cured monolayer of the resin composition. The resulting cured monolayer was cut into a length of 1.5 cm x 3 cm and rolled up to create a cylindrical sample with a diameter of 2 mm and a length of 1.5 cm. This sample was measured in indentation mode using a thermal analyzer TMA / SS6600 (manufactured by Hitachi High-Tech Science Corporation). The glass transition temperature was calculated from the inflection point of the obtained TMA curve. The coefficient of linear thermal expansion (CTE) was calculated as the rate of change in sample length from a temperature 80°C lower than the glass transition temperature of each cured product to a temperature 30°C lower than the glass transition temperature according to the following formula (X): CTE (1 / K) = ((sample length (m) at Tg - 30°C) - (sample length (m) at Tg - 80°C)) / (sample length (m) before measurement × 50 (K)) Formula (X)

[0118] (2) Measurement of Thermal Decomposition Temperature Approximately 15 mg of a single film of the cured film used in the measurements of glass transition temperature and linear thermal expansion coefficient was placed in a standard aluminum container and measured using a thermogravimetric analyzer (TGA-50, manufactured by Shimadzu Corporation). The measurement conditions were as follows: after holding at 120°C for 30 minutes, the temperature was increased to 500°C at a rate of 5°C / min. The temperature at which the weight decreased by 1% was read from the obtained weight loss curve, and this temperature was defined as the 1% weight loss temperature.

[0119] (3) Evaluation of Laminate Adhesion Resin compositions 1 to 43 were applied to a 500 μm-thick 4-inch silicon substrate by adjusting the rotation speed with a spin coater to achieve a cured thickness of 8 μm. The substrate was then heat-treated at 120°C for 3 minutes and dried, followed by heat treatment at 250°C for 30 minutes to cure the resin. Next, a 4-inch glass substrate (manufactured by Corning Japan Inc., product name: EX-G) was placed on top of the substrate, and the upper and lower plates were pressure-bonded at a pressure of 1.0 MPa for 5 minutes using a vacuum bonder (manufactured by Mikado Technos Co., Ltd.) set at 200°C, to obtain a laminate in which a cured product was formed between the glass substrate and the silicon substrate. Resin compositions 1 to 43 were also diluted with solvent as needed and applied to a 4-inch silicon substrate using a spin coater to achieve a cured film thickness of 2.0 μm. A laminate with a cured film thickness of 2.0 μm was prepared using the same method as for preparing the laminate with a cured film thickness of 8.0 μm described above. These laminates were viewed from the glass substrate side, and the adhesive area was confirmed visually. Those in which 90% or more of the substrate area was bonded were rated A; similarly, those in which 80% or more but less than 90% was rated B; those in which 70% or more but less than 80% was rated C; those in which 50% or more but less than 70% was rated D; and those in which less than 50% was rated E.

[0120] (4) Evaluation of heat resistance of laminate The laminate having a cured film thickness of 2.0 μm, which was prepared for the evaluation of the adhesiveness of the laminate, was placed on a hot plate heated to 300° C. with the silicon substrate surface in contact with the hot plate and heated for 3 minutes. Thereafter, the laminate was transferred to a tray and cooled to room temperature, and then the bonding area was evaluated using the same evaluation method as in (3).

[0121] The names of the acid dianhydrides, diamines, additives, and solvent abbreviations used in the following preparations are as follows: BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride. This is the acid dianhydride that gives the structure of the acid dianhydride residue (A1) after polymerization. (Mitsubishi Chemical Corporation) PMDA: pyromellitic dianhydride (Daicel Corporation) BSAA: 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (SHPP Japan LLC) 6FDA: 4,4'-(hexafluoroisopropylidene)diphthalic dianhydride (Merck Ltd.) ODPA: 3,3',4,4'-diphenylethertetracarboxylic dianhydride (Toho Chemical Industry Co., Ltd.) Benzidine: 4,4'-diaminobiphenyl. This is the diamine that gives the structure of the diamine residue (A2) after polymerization. (Manufactured by Tokyo Chemical Industry Co., Ltd.) m-TB: 2,2'-dimethyl-4,4'-diaminobiphenyl. After polymerization, a diamine gives a diamine residue (A2) having a structure represented by formula (6). (Manufactured by Wakayama Seika Kogyo Co., Ltd.) LP-7100: tetramethyl-1,3-bis(3-aminopropyl)disiloxane. A diamine having a silicon atom and giving a diamine residue (A3) structure after polymerization. n in formula (5) is 1. (Product name: manufactured by Shin-Etsu Chemical Co., Ltd.) APPS2: α,ω-bis(3-aminopropyl)polydimethylsiloxane. A diamine having a silicon atom and giving a diamine residue (A3) structure after polymerization. The number average molecular weight is 860, and the average n in formula (5) is 9. DDS: 3,3'-diaminodiphenyl sulfone. (Manufactured by Konishi Chemical Industry Co., Ltd.) BAHF: 2,2-bis(3-amino-4 hydroxyphenyl)hexafluoropropane. (Manufactured by Merck Electronics Co., Ltd.) NMP: N-methylpyrrolidone. Solvent used in polymerization and blending. (Manufactured by Mitsubishi Chemical Corporation, viscosity: 1.70 mPa·s) CHN: Cyclohexanone. Solvent used in polymerization and blending. (Manufactured by Toyo Gosei Co., Ltd., viscosity: 1.97 mPa·s) DMI: Dimethylimidazolidinone. Solvent used in polymerization and blending. (Manufactured by Fuji Film Wako Co., Ltd., viscosity: 2.63 mPa·s) DAA: Diacetone alcohol. Solvent used in polymerization and blending. (Manufactured by Tokyo Chemical Industry Co., Ltd., viscosity: 2.90 mPa·s) DPM: Dipropylene glycol monomethyl ether.Solvent used in polymerization and compounding (manufactured by Tokyo Chemical Industry Co., Ltd., viscosity: 3.47 mP·s) KBM-403: 3-glycidoxypropyltrimethoxysilane. Silane coupling agent (product name: manufactured by Shin-Etsu Chemical Co., Ltd.) KBM-1083: 7-octenyltrimethoxysilane. Silane coupling agent having a structure represented by formula (9). (product name: manufactured by Shin-Etsu Chemical Co., Ltd.) KBM-4803: 8-glycidoxyoctyltrimethoxysilane. Silane coupling agent corresponding to formula (8). (product name: manufactured by Shin-Etsu Chemical Co., Ltd.) KBM-5803: 8-methacryloxyoctyltrimethoxysilane. Silane coupling agent having a structure represented by formula (10). (product name: manufactured by Shin-Etsu Chemical Co., Ltd.) KBM-6803: N-2-(aminoethyl)-8-aminooctyltrimethoxysilane. A silane coupling agent having a structure represented by formula (11). (Product name: manufactured by Shin-Etsu Chemical Co., Ltd.) MEK-EC-2030Y: Organosilica sol dispersed in methyl ethyl ketone (SiO 2 Concentration: 30 wt%) (product name: manufactured by Nissan Chemical Co., Ltd.)

[0122] <Production Example 1> In a reaction vessel equipped with a thermometer, a dry nitrogen inlet, a heating / cooling device using hot water and cooling water, and a stirrer, 18.5 g of LP-7100, 80.7 g of DDS, and 36.6 g of BAHF, which are diamine components, were dissolved together with 562.7 g of NMP. Then, 22.7 g of BPDA and 131.8 g of ODPA, which are acid dianhydride components, were added, and the mixture was stirred at 60°C for 4 hours, and then reacted at 130°C for 2 hours. After completion of polymerization, NMP was added to adjust the concentration to 30 wt% solids, and PI-1, a polymerization solution of polyimide / polyamic acid copolymer, was prepared.

[0123] <Production Examples 2 to 27> PI-2 to PI-27, which are polymerization solutions of polyimide / polyamic acid copolymers, were prepared in the same manner as in Example 1, except that the acid anhydride, diamine, and solvent were changed to the compositions and amounts added shown in Tables 1 to 3.

[0124] Examples 1 to 37, Comparative Examples 1 to 6 Resin compositions 1 to 43 were prepared by mixing and stirring a silane coupling agent, inorganic particles, and a solvent into the polymerization solutions of the polyimide / polyamic acid copolymers obtained in Production Examples 1 to 27 according to the contents of Tables 4 to 6. The resin compositions were filtered through a PTFE filter with a pore size of 0.5 μm. Using these resin compositions, evaluation samples were prepared by the methods described above, and various evaluations were performed. The evaluation results are shown in Tables 7 to 9.

[0125]

[0126]

[0127]

[0128]

[0129]

[0130]

[0131]

[0132]

[0133]

[0134] [Comparative Example 1, Examples 1 and 7] In Example 1, the resin (A) contained at least one of the acid dianhydride residues (X1) and (X2) and the diamine residues (Y1) and (Y2) in a total of 100 mol % relative to the total of 100 mol %. Therefore, the linear thermal expansion coefficient was lower than that of Comparative Example 1. This reduced warping of the substrate due to heat treatment, thereby reducing peeling of the laminate after heat treatment. Furthermore, Example 7 contained at least one of the acid dianhydride residues (A1) and the diamine residues (A2) in a total of 15 mol % or more. This further reduced the linear thermal expansion coefficient, thereby further improving peeling of the laminate after heat treatment.

[0135] [Comparative Example 2, Examples 2 and 8] In Example 2, the resin (A) contained at least one of the acid dianhydride residues (X1) and (X2) and the diamine residues (Y1) and (Y2) in a total of 100 mol %. Therefore, the glass transition temperature was more appropriate than in Comparative Example 2. This resulted in good initial adhesion of the laminate. Furthermore, in Example 8, the initial adhesion of the laminate was further improved, particularly in thin films, by limiting the total content of at least one of the acid dianhydride residues (A1) and the diamine residues (A2) to 30 mol % or less.

[0136] [Comparative Example 3, Examples 3 and 9] In Example 3, the proportion of all Si atoms contained in the resin (A) was 0.5 parts by mass or more relative to 100 parts by mass of the resin (A), and therefore, the laminate was easier to attach to the entire surface of the substrate compared to Comparative Example 3. In Example 9, the proportion of all Si atoms contained in the resin (A) was 2.0 parts by mass or more relative to 100 parts by mass of the resin (A), and therefore, the initial adhesiveness of the laminate was further improved.

[0137] [Comparative Example 4, Examples 4 and 10] In Example 4, the proportion of all Si atoms contained in the resin (A) was 5.0 parts by mass or less relative to 100 parts by mass of the resin (A), and therefore the thermal stability was excellent and the 1% weight loss temperature was improved compared to Comparative Example 4. As a result, when the laminate was heat-treated, cloudiness and peeling due to decomposition of the Si component were suppressed. In Example 10, the proportion of all Si atoms contained in the resin (A) was 4.0 parts by mass or less relative to 100 parts by mass of the resin (A), and therefore the coefficient of linear thermal expansion was further reduced, and the adhesion of the laminate after heat treatment was improved.

[0138] [Comparative Example 5, Examples 5, 11, 30, and 32] In Example 5, the resin (A) contains 1.0 mol% or more of the diamine residue (A3) relative to a total of 100 mol% of the acid dianhydride residues (X1) and (X2) and the diamine residues (Y1) and (Y2) contained in the resin (A). Therefore, the Si component involved in adhesion is distributed throughout the cured product, and the initial adhesion of the laminate could be improved compared to Comparative Example 5. Furthermore, in Examples 11, 30, and 32, the resin (A) contains 2.0 mol% or more of the diamine residue (A3) relative to a total of 100 mol% of the acid dianhydride residues (X1) and (X2) and the diamine residues (Y1) and (Y2) contained in the resin (A). Therefore, the Si component is distributed more uniformly, and the adhesion of the laminate near the periphery of the substrate could be further improved.

[0139] [Comparative Example 6, Examples 6, 12, and 13] In Example 6, the resin (A) contains 20 mol% or less of the diamine residue (A3) relative to the total of 100 mol% of the acid dianhydride residues (X1) and (X2) and the diamine residues (Y1) and (Y2) contained in the resin (A). Therefore, heat resistance is improved, and unlike Comparative Example 6, the cloudiness of the film caused by decomposition gases can be suppressed during the heat treatment of the laminate. Furthermore, in Examples 12 and 13, the resin (A) contains 17 mol% or less of the diamine residue (A3) relative to the total of 100 mol% of the acid dianhydride residues (X1) and (X2) and the diamine residues (Y1) and (Y2) contained in the resin (A). Therefore, the linear thermal expansion coefficient and glass transition temperature are optimized, and excessive softening of the film during heat treatment can be suppressed. As a result, the adhesion of the laminate after heat treatment can be greatly improved.

[0140] Example 29 contains m-TB represented by formula (6) as the diamine residue (A2), and thus the stability of the polymer in the varnish and the uniformity of the coating film thickness were improved compared to Example 11. As a result, the adhesiveness, particularly in thin films, was improved.

[0141] In Example 31, the solvent constituting the resin component was CHN alone, which had a viscosity of 1.8 mPa s or more, thereby improving the edge coating properties when forming a coating film. As a result, the adhesiveness of the laminate, particularly in the case of a thin film, was improved compared to Examples 11 and 30.

[0142] In Examples 33 and 34, the use of DAA or DMI, which has a viscosity of 3.1 mPa s or less, as the solvent for the resin component improved the coatability when forming the coating film. As a result, the adhesion of the laminate was improved compared to Examples 11 and 30.

[0143] Example 35 contains m-TB represented by formula (6) as the diamine residue (A2), and thus the stability of the polymer in the varnish was improved and the thickness uniformity of the coating film was improved compared to Examples 11 and 34. As a result, the adhesiveness, particularly in thin films, was improved.

[0144] Example 36 In Example 36, the diamine residue (A3) contained LP-7100, which has a repeating unit number n=1, and thus the heat resistance was improved compared to Examples 33 and 34. As a result, the adhesiveness of the laminate after heat treatment was significantly improved.

[0145] Example 37 Example 37 had m-TB represented by formula (6) as the diamine residue (A2) and LP-7100 with a repeating unit number n = 1 as the diamine residue (A3), thereby improving the in-plane uniformity and heat resistance of the coating film compared to Examples 35 and 36. As a result, the adhesion of the laminate and the adhesion of the laminate after heat treatment were improved. Furthermore, by using DMI with a viscosity of 1.8 mPa s or more as the solvent constituting the resin element, the film thickness uniformity at the edge of the coating film was improved compared to Example 13. As a result, adhesion was improved, especially in thin films.

[0146] Example 13 contains 2,2'-dimethyl-4,4'-diaminobiphenyl, which has the structure of formula (6), as the diamine residue (A2), and thus both the initial adhesiveness and the adhesiveness after heat treatment of the laminate were improved compared to Example 12. Furthermore, the number of repeating units n of the diamine residue (A3) was 1, and thus both the heat resistance and adhesiveness were improved compared to Example 29.

[0147] [Examples 14 to 18 and 23] In Examples 14 to 18, the resin compositions contained a silane coupling agent, and thus the initial adhesion of the laminate was improved compared to Example 12. Similarly, in Example 23, the initial adhesion of the laminate was improved compared to Example 13, particularly in the case of a thin film.

[0148] [Examples 19 to 22 and 24] In Examples 19 to 22 and 24, the resin composition contains a silane coupling agent represented by formula (7), and thus the initial adhesion of the laminate and the adhesion after heat treatment can be further improved compared to Example 17.

[0149] [Examples 25 to 27] In Examples 25 to 27, the resin composition contained inorganic particles, and thus the coefficient of linear thermal expansion was reduced compared to Examples 12 and 13, and the decrease in adhesiveness due to heat treatment of the laminate was significantly reduced.

[0150] [Example 28] In Example 28, the resin composition contained both the silane coupling agent represented by formula (7) and inorganic particles, and thus it was possible to efficiently suppress both peeling due to insufficient adhesion and peeling during heat treatment due to warping of the substrate. As a result, it was possible to further reduce peeling of the laminate after heat treatment compared to Example 24.

[0151] Although the present invention has been described in detail with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on a Japanese patent application (Patent Application No. 2023-054038) filed on March 29, 2023, the entirety of which is incorporated by reference. All references cited herein are incorporated in their entirety.

[0152] 1 Monolithic LED element 2 Circuit substrate 10 First LED layer 20 Second LED layer 30 Third LED layer 110 First sapphire substrate 111 First n-type GaN layer 112 First light-emitting layer 113 First p-type GaN layer 114 First transparent electrode 120 Second sapphire substrate 121 Second n-type GaN layer 122 Second light-emitting layer 123 Second p-type GaN layer 124 Second transparent electrode 130 Third sapphire substrate 131 Third n-type GaN layer 132 Third light-emitting layer 133 Third p-type GaN layer 134 Third transparent electrode 220 Second adhesive layer 230 Third adhesive layer 310 Passivation layer 320 Electrode

Claims

1. A resin composition containing a resin (A) having at least one structural unit selected from the structural units represented by formula (1) and the structural units represented by formula (2), and a solvent, wherein, relative to a total of 100 mol % of the acid dianhydride residues (X1) and (X2) and the diamine residues (Y1) and (Y2) contained in the resin (A), the resin (A) contains at least one of the acid dianhydride residue (A1) having a structure represented by formula (3) and the diamine residue (A2) having a structure represented by formula (4), in a total amount of 10 mol % to 40 mol %, the resin (A) contains 1.0 mol % to 20 mol % of the diamine residue (A3) having a structure represented by formula (5), and the proportion of all Si atoms contained in the resin (A) is 0.5 parts by mass to 5.0 parts by mass per 100 parts by mass of the resin (A). (In formula (1) and formula (2), X 1 and X 2 each independently represents a tetravalent acid dianhydride residue having 4 to 50 carbon atoms; Y 1 and Y 2 R each independently represents a divalent diamine residue having 2 to 100 carbon atoms. 1 and R 2 each independently represents a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, an alkylsilyl group having 1 to 10 carbon atoms, an alkali metal atom, an ammonium group, an imidazolium group, or a pyridinium group. (In formulas (3) to (5), R 3 ~R 16 R each independently represents a hydrogen atom, a monovalent organic group having 1 to 20 carbon atoms, a hydroxyl group, or a halogen atom. 17 ~R 20 R each independently represents an alkyl group having 1 to 30 carbon atoms, an alkoxy group having 1 to 30 carbon atoms, a phenyl group, or a phenoxy group. 21 and R 22 each independently represents an alkylene group or a phenylene group having 1 to 30 carbon atoms, and n represents an integer of 1 to 20. * 3a and * 3b represents a bonding site connected to an imide group in the structural unit represented by formula (1), or * 3a represents a bonding site connected to the carbon atom of the amide bond in the structural unit represented by formula (2), * 3b represents a bonding site connecting to a carbon atom of a carboxylic acid or a carboxylate in the structural unit represented by formula (2). * 4, and * 5 represents a bonding site connected to the nitrogen atom of the imide group in the structural unit represented by formula (1) or the amide bond in the structural unit represented by formula (2).

2. The resin composition according to claim 1, wherein the diamine residue (A2) is a diamine residue having a structure represented by formula (6). (In formula (6), * 6 represents a bonding site connected to the nitrogen atom of the imide group in the structural unit represented by formula (1) or the amide bond in the structural unit represented by formula (2).

3. The resin composition according to claim 1, wherein in the diamine residue (A3), n in the formula (5) is 1.

4. The resin composition according to claim 1, wherein the solvent contained in the resin composition has a viscosity of 1.8 mPa·s or more and 3.1 mPa·s or less.

5. The resin composition according to claim 1 or 2, further comprising a silane coupling agent.

6. The resin composition according to claim 5, wherein the silane coupling agent contains a compound represented by formula (7). (In formula (7), R 23 R represents an alkylene group having 5 to 10 carbon atoms. 24 each independently represents an alkyl group having 1 to 5 carbon atoms; and Z represents a hydrogen atom or a group represented by any one of the following formulas (8) to (14). (In formulas (8) to (14), R 25 ~R 31 each independently represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, a hydroxyl group, or a halogen atom. * 8~ * 14 is R in formula (7) 23 It represents the binding site with 7. The resin composition according to claim 1 or 2, further comprising inorganic particles.

8. A cured product obtained by curing the resin composition according to any one of claims 1 to 4.

9. A laminate comprising the cured product according to claim 8.

10. The laminate according to claim 9, wherein the thickness of the cured product is 0.5 μm or more and 8.0 μm or less.

11. The laminate according to claim 10, which has a plurality of layers made of the cured product.

12. The stack according to claim 10, wherein the stack comprises a compound semiconductor layer.

13. A semiconductor device comprising the laminate according to claim 10.

14. A method for manufacturing a semiconductor device, comprising at least one of the steps of thinning the laminate according to claim 10 and dividing the laminate according to claim 10 into individual pieces.

Citation Information

Patent Citations

  • Polyimide film, layered body, surface material for display, touch panel member, liquid crystal display device, and organic electroluminescent display device

    JP2020002196A

  • Polyimide resin, varnish, and polyimide film

    WO2020100904A1

  • Polyimide precursor and polyimide resin composition

    WO2020241523A1