Solid electrolyte, solid electrolyte layer, and solid electrolyte battery
The development of a solid electrolyte with a tailored Raman spectrum and elemental composition addresses the limitations in ionic conductivity and rate characteristics of existing halide-based electrolytes, enhancing battery performance by forming a conducive path for lithium ions and reducing electrochemical reactions.
Patent Information
- Application Number
- PCT/JP2024/011934
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-03
AI Technical Summary
Current solid electrolytes, particularly halide-based ones like Li3ScCl6 and Li2Zr(SO4)Cl4, face limitations in ionic conductivity and charging/discharging rate characteristics, necessitating an improvement in their configuration to enhance performance without altering their composition.
A solid electrolyte with a specific Raman spectrum profile, characterized by peaks within certain ranges and intensity ratios, is developed, incorporating elements like Zr, S, and halides, which forms a conduction path that suppresses local electrochemical reactions, thereby improving rate characteristics.
The optimized solid electrolyte achieves enhanced ionic conductivity and rate characteristics, leading to improved performance in solid electrolyte batteries by forming a conduction path where lithium ions are less likely to be bound, thus suppressing non-uniform electrochemical reactions.
Smart Images

Figure JP2024011934_03102024_PF_FP_ABST
Abstract
Description
Solid electrolyte, solid electrolyte layer and solid electrolyte battery
[0001] The present invention relates to a solid electrolyte, a solid electrolyte layer, and a solid electrolyte battery. This application claims priority to Japanese Patent Application No. 2023-058580, filed on March 31, 2023, the contents of which are incorporated herein by reference.
[0002] In recent years, electronics technology has made remarkable progress, leading to efforts to make portable electronic devices smaller, lighter, thinner, and more multifunctional. Accordingly, there is a strong demand for batteries, which serve as the power source for electronic devices, to be smaller, lighter, thinner, and more reliable. Solid electrolyte batteries, which use solid electrolytes as the electrolyte, have attracted attention. Known solid electrolytes include oxide-based solid electrolytes, sulfide-based solid electrolytes, complex hydride-based solid electrolytes, and halide-based solid electrolytes.
[0003] For example, Non-Patent Document 1 discloses that a halide-based solid electrolyte, Li 3 ScCl 6 It is described that the ionic conductivity of the cation exchanger is 3 mS / cm, and the potential window on the reduction side is 0.91 V (V vs. Li / Li + ) is stated.
[0004] Japanese Patent Application Laid-Open No. 2022-122849
[0005] Jianwen Liang et al., J. Am. Chem. Soc., 2020, 142, 7012-7022.RJH Clark, “The impact of Laser-Raman spectroscopy on inorganic chemistry”, The SPEX Speaker Vol. XVIII, No. 1 (March, 1973)
[0006] Halide-based solid electrolytes are said to have higher ionic conductivity than oxide-based solid electrolytes, sulfide-based solid electrolytes, complex hydride-based solid electrolytes, etc. 3 ScCl 6Although the ionic conductivity of SiO2 (3 mS / cm) is high, it is subject to various limitations, and there are cases where the properties described in Non-Patent Document 1 are not fully realized or other materials have to be selected. Therefore, there is a demand for a configuration that can relatively improve the ionic conductivity of solid electrolytes with similar structures.
[0007] Li, known as a halide-based solid electrolyte 2 ZrCl 6 and Li 2 Zr(SO 4 ) Cl 4 (See, for example, Patent Document 1) uses Zr, which is abundant in the earth's crust, as the central metal, and is a solid electrolyte material that is advantageous in terms of resource availability and cost. However, its ionic conductivity is 4x10 -4 S / cm 2 , and the charge / discharge rate characteristics of a battery using this solid electrolyte are insufficient.
[0008] The present inventors have conducted extensive research and have succeeded in improving the rate characteristics without changing the composition of the halide-based solid electrolyte, thereby completing the present invention.
[0009] The present invention has been made in view of the above-mentioned problems, and has an object to provide a solid electrolyte capable of improving rate characteristics, a solid electrolyte layer using the same, and a solid electrolyte battery.
[0010] In order to solve the above problems, the present invention provides the following means.
[0011] The solid electrolyte according to the first aspect of the present invention is represented by the formula (1), and has a Raman spectrum measured at an excitation wavelength of 532 nm of 900-1250 cm -1 In the range 950 to 1025 cm -1 Peak a with a peak top in the range 1026-1110 cm -1 a solid electrolyte having two or more peaks, a A b Zr c B d (SO 4 ) e Cl f X g... (1) (In the formula, A is at least one element selected from alkali metals and alkaline earth metals; B is at least one element selected from the group consisting of Na, K, Rb, Cs, Mg, Ca, Sr, Ba, B, Si, Al, Ti, Cu, Sc, Y, Zr, Nb, Ag, In, Sn, Sb, Hf, Ta, W, Au, and Bi; X is at least one element selected from the group consisting of F, Br, and I; and 0.5≦a<6, 0≦b<6, 0<c<2, 0≦d<1, 0<e<3, 0<f≦5, and 0≦g<5.)
[0012] The solid electrolyte according to the second aspect of the present invention is the solid electrolyte according to the first aspect, which has a Raman spectrum of 900-1250 cm -1 The intensities of peak a and peak b are Ia and Ib, respectively, relative to the baseline, and Ia>Ib.
[0013] A solid electrolyte layer according to a third aspect of the present invention includes the solid electrolyte according to any one of the first and second aspects.
[0014] A solid electrolyte battery according to a fourth aspect of the present invention includes a solid electrolyte layer, a positive electrode, and a negative electrode, and at least one of the positive electrode and the negative electrode contains the solid electrolyte according to any one of the first and second aspects.
[0015] A solid electrolyte battery according to a fifth aspect of the present invention includes the solid electrolyte layer of the third aspect, a positive electrode, and a negative electrode.
[0016] The solid electrolyte of the present invention can provide a solid electrolyte, a solid electrolyte layer, and a solid electrolyte battery having high rate characteristics.
[0017] 1 is a diagram showing a Raman spectrum of Example 1 according to the present embodiment; FIG. 2 is a diagram showing a Raman spectrum of Example 2 according to the present embodiment; FIG. 3 is a diagram showing a Raman spectrum of Comparative Example 1 according to the present embodiment; FIG. 4 is a cross-sectional schematic diagram of a solid electrolyte battery according to the present embodiment.
[0018] The present embodiment will be described in detail below with reference to the accompanying drawings. The drawings used in the following description may show characteristic portions enlarged for the sake of clarity, and the dimensional proportions of each component may differ from the actual proportions. The materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not limited thereto. Appropriate modifications may be made within the scope of the present invention.
[0019] "Solid electrolyte" A solid electrolyte is a substance that can move ions when an external electric field is applied. If the ionic conductivity of a solid electrolyte is high, the exchange of ions in the solid electrolyte battery becomes smoother, and the internal resistance becomes smaller.
[0020] The solid electrolyte is Li a A b Zr c B d (SO 4 ) e Cl f X g The solid electrolyte may contain a halide-based solid electrolyte represented by the formula (1) above, as well as a material derived from the raw material powder. The material derived from the raw material powder may be, for example, Li 2 SO 4 is.
[0021] The solid electrolyte may be in the form of a powder (particles) or a sintered body obtained by sintering the powder. The solid electrolyte may also be a compact obtained by compressing the powder, a compact obtained by molding a mixture of the powder and a binder, or a coating formed by applying a coating containing the powder, a binder, and a solvent and then heating to remove the solvent. The main structure of the solid electrolyte may be amorphous or crystalline.
[0022] In formula (1), A is at least one element selected from alkali metals and alkaline earth metals. A substitutes for a portion of the Li ions. A is, for example, Li, Na, Ca, or K. When A is Na, Ca, or K, the potential window on the reduction side of the solid electrolyte is widened. From the viewpoint of adjusting the potential window, it is preferable that b satisfies 0≦b<6.
[0023] In formula (1), B is an element that is contained as needed. B is at least one element selected from the group consisting of Na, K, Rb, Cs, Mg, Ca, Sr, Ba, B, Si, Al, Ti, Cu, Sc, Y, Zr, Nb, Ag, In, Sn, Sb, Hf, Ta, W, Au, and Bi. When the solid electrolyte contains the element B, d preferably satisfies 0≦d<1, from the viewpoint of adjusting the ionic conductivity and the potential window.
[0024] In formula (1), it is preferable that a satisfies 0.5≦a<6 in terms of adjusting the carrier concentration.
[0025] In formula (1), c preferably satisfies 0<c<2 in terms of adjusting the potential window of the solid electrolyte.
[0026] In formula (1), e preferably satisfies 0<e<3 from the viewpoint of adjusting the potential window of the solid electrolyte. When e is 0.1 or more, (SO 4 If the content is too large, the space for carrier ions to move becomes narrower, which may result in a decrease in the ionic conductivity of the solid electrolyte. From the viewpoint of suppressing this, it is preferable that c is smaller than 3 and not more than 2.5.
[0027] In formula (1), SO 4 In addition, the anion may have at least one group selected from the group consisting of OH, BO 2 , B.O. 3 , B.O. 4 , B 3 O 6 , B 4 O 7 , CO 3 , NO 3 , AlO 2 , SiO 3 , SiO 4 , Si 2 O 7 , Si 3 O 9 , Si 4 O 11 , Si 6 O 18 , P.O. 3 , P.O.4 , P 2 O 7 , P 3 O 10 , S.O. 3 , S.O. 5 , S 2 O 3 , S 2 O 4 , S 2 O 5 , S 2 O 6 , S 2 O 7 , S 2 O 8 , B.F. 4 , P.F. 6 ,BOB,(COO) 2 , N, AlCl 4 , C.F. 3 SO 3 , C.H. 3 COO, CF 3 COO,OOC-(CH 2 ) 2 -COO,OOC-CH 2 -COO, OOC-CH(OH)-CH(OH)-COO, OOC-CH(OH)-CH 2 -COO, C 6 H 5 SO 3 , OOC-CH=CH-COO, C(OH)(CH 2 COOH) 2 COO, AsO 4 , Bio 4 , CrO 4 , MnO 4 , PtF 6 , PtCl 6 , PtBr 6 , PtI 6 , SbO 4 , SeO 4 , TeO 4 , HCOO, CH 3 At least one group selected from the group consisting of COO, O (BOB is bis(oxalato)borate, OOC—(CH 2 ) 2 -COO is succinate, OOC-CH 2-COO is malonate, OOC-CH(OH)-CH(OH)-COO is tartrate, OOC-CH(OH)-CH 2 -COO is malate, C 6 H 5 SO 3 is the benzenesulfonate, OOC-CH=CH-COO is the fumarate, OOC-CH=CH-COO is the maleate, and C(OH)(CH 2 COOH) 2 COO is citrate. 4 In addition, by selecting the above groups as the anion, it is preferable from the viewpoint of adjusting the ionic conductivity and the potential window.
[0028] In formula (1), f preferably satisfies 0<f≦5 in terms of adjusting the potential window of the solid electrolyte.
[0029] In formula (1), X is at least one selected from the group consisting of F, Br, and I. X has a large ionic radius per valence. The inclusion of X in the solid electrolyte adjusts the conductivity, oxidation resistance, and reduction resistance of lithium ions in the solid electrolyte. From the viewpoint of improving the balance between the oxidation resistance and reduction resistance of the solid electrolyte, X preferably contains F. From the viewpoint of improving the reduction resistance of the solid electrolyte, X preferably contains I. Two or more selected from the group consisting of F, Br, and I may be included. From the viewpoint of adjusting the ionic conductivity and the potential window, it is preferable to satisfy 0≦g<5.
[0030] The solid electrolyte may be, for example, Li 2 ZrSO 4 Cl 4 , Li 3 YSO 4 Cl 4 , Li 3 ScSO 4 Cl 4 , Li 3 InSO 4 Cl 4 is.
[0031] In Raman spectroscopy, light is incident on a material and the material is evaluated based on the Raman scattered light, which has a wavelength different from that of the incident light. Because the wavelength difference between the Raman scattered light and the incident light corresponds to the vibrational energy of the material, various physical properties of the material can be investigated from the Raman spectrum. Therefore, it is possible to capture characteristics of amorphous materials that cannot be investigated by X-ray diffraction. In highly crystalline solids with a regular crystal lattice, the peaks corresponding to each vibrational energy are sharp, while broad peaks reflect crystallinity disorder (promotion of an amorphous structure). Furthermore, because the wavelength difference between the Raman scattered light and the incident light corresponds to the vibrational energy of the material, the Raman spectrum reflects information about the molecular structure and differences in the crystalline structure. After extensive research, the inventors attempted to improve the rate performance of solid electrolytes without changing their composition, and discovered that the characteristics of the Raman spectrum correlate with the rate performance, leading to the invention.
[0032] The solid electrolyte according to this embodiment has a Raman spectrum measured at an excitation wavelength of 532 nm, which has a range of 900-1250 cm -1 In the range 950 to 1025 cm -1 Peak a with a peak top in the range 1026-1110 cm -1 The composition has two or more peaks, namely, peak a having a peak top at 10 ...
[0033] The solid electrolyte according to this embodiment has a Raman spectrum measured at an excitation wavelength of 532 nm, which shows a Raman spectrum of 900-1250 cm -1 When the intensities of peak a and peak b are Ia and Ib, respectively, relative to the baseline, the straight line connecting the above is Ia > Ib. Although it is not certain, a composition having two or more peaks and satisfying the peak intensity relationship is preferable from the viewpoint of forming a conduction path in which lithium ions are less likely to be constrained. Since locally non-uniform electrochemical reactions can be further suppressed, the rate characteristics of the solid electrolyte battery are further improved.
[0034] The solid electrolyte according to this embodiment has a peak energy of 170±0.5 eV (the chemical state of sulfur is SO ) in X-ray photoelectron spectroscopy (XPS). 4 ) and 532±0.5 eV (corresponding to the chemical state of oxygen being SO 4 It is preferable that the sulfur and oxygen in the solid electrolyte are strongly bonded to each other and have a peak at SO 4 By maintaining the structure and being present in the solid electrolyte material, it is possible to form a conduction path where lithium ions are less likely to be constrained, which is advantageous. This suppresses locally non-uniform electrochemical reactions, thereby improving the rate characteristics of solid electrolyte batteries.
[0035] "Solid Electrolyte Battery" FIG. 4 is a cross-sectional schematic diagram of a solid electrolyte battery 100 according to this embodiment. The solid electrolyte battery 100 shown in FIG. 4 includes a power generating element 40 and an exterior body 50. The exterior body 50 covers the periphery of the power generating element 40. The power generating element 40 is connected to the outside via a pair of connected terminals 60, 62. Although FIG. 4 shows a stacked-type battery, a wound-type battery may also be used. The solid electrolyte battery 100 is used, for example, in laminate batteries, prismatic batteries, cylindrical batteries, coin batteries, button batteries, etc.
[0036] <Power generating element> The power generating element 40 includes a solid electrolyte layer 10, a positive electrode 20, and a negative electrode 30. The power generating element 40 is charged or discharged by the exchange of ions between the positive electrode 20 and the negative electrode 30 via the solid electrolyte layer 10 and the exchange of electrons via an external circuit.
[0037] (Solid Electrolyte Layer) The solid electrolyte layer 10 is a layer containing the solid electrolyte according to this embodiment. The solid electrolyte layer 10 may consist solely of the solid electrolyte according to this embodiment, or may be used together with a support such as a binder or nonwoven fabric. The binder may be the same as that used in the electrodes. The ratio of the binder to the solid electrolyte is preferably less than 30% by volume to avoid impeding lithium ion conduction. A support such as nonwoven fabric may be used to suppress locally uneven electrochemical reactions due to cracks, etc. The material of the support such as nonwoven fabric may be any insulating material such as resin, ceramic, or glass used as the binder, and preferably has an aperture ratio of 85% or more. The solid electrolyte layer 10 is sandwiched between the positive electrode 20 and the negative electrode 30. The solid electrolyte layer 10 contains a solid electrolyte capable of transferring ions when an external voltage is applied. For example, the solid electrolyte conducts lithium ions and inhibits the transfer of electrons.
[0038] The solid electrolyte layer 10 may be composed of, for example, only the solid electrolyte according to this embodiment, or may be used together with other solid electrolytes as needed. They may be mixed or may be used in two or more separate layers. Here, the other solid electrolytes are those that conduct lithium ions and inhibit the movement of electrons, such as oxide-based solid electrolytes, halide-based solid electrolytes, sulfide-based solid electrolytes, complex hydride-based solid electrolytes, and ion-conductive polymers.
[0039] The solid electrolyte layer 10 contains, for example, the above-mentioned solid electrolyte. The above-mentioned solid electrolyte contained in the positive electrode 20 or the negative electrode 30 may be the same as or different from the solid electrolyte contained therein.
[0040] 4, the positive electrode 20 has a plate-shaped (foil-shaped) positive electrode current collector 22 and a positive electrode mixture layer 24. The positive electrode mixture layer 24 is in contact with at least one surface of the positive electrode current collector 22.
[0041] The positive electrode current collector 22 may be made of any electronically conductive material that is resistant to oxidation during charging and corrosion. Examples of the positive electrode current collector 22 include metals such as aluminum, stainless steel, nickel, and titanium, alloys thereof, and conductive resins. The positive electrode current collector 22 may be in the form of powder, foil, punching, or expanded.
[0042] The positive electrode mixture layer 24 contains a positive electrode active material, and optionally a solid electrolyte, a binder, and a conductive additive.
[0043] The positive electrode active material is not particularly limited as long as it can reversibly absorb and release lithium ions and insert and extract them (intercalate and deintercalate), and any positive electrode active material used in known solid electrolyte batteries can be used. Examples of the positive electrode active material include lithium-containing metal oxides and lithium-containing metal phosphates.
[0044] The lithium-containing metal oxide is, for example, lithium cobalt oxide (LiCoO 2 ), lithium nickel oxide (LiNiO 2 ), lithium manganese spinel (LiMn 2 O 4 ), and general formula: LiNixCoyMnzO 2 A composite metal oxide represented by (x + y + z = 1), a lithium vanadium compound (LiVOPO 4 , Li 3 V 2 (P.O. 4 ) 3 ), olivine-type LiMPO 4 (wherein M represents at least one selected from Co, Ni, Mn, and Fe), lithium titanate (Li 4 Ti 5 O 12 ) etc.
[0045] The positive electrode active material may not contain lithium. Examples of such a positive electrode active material include lithium-free metal oxides (MnO 2 , V 2 O 5 etc.), lithium-free metal sulfides (MoS 2 etc.), lithium-free fluorides (FeF3 , V.F. 3 When a positive electrode active material that does not contain lithium is used, the negative electrode is doped with lithium ions in advance, or a negative electrode containing lithium ions is used.
[0046] The solid electrolyte contained in the positive electrode 20 is, for example, the above-mentioned solid electrolyte. The solid electrolyte contained in the positive electrode 20 may be a halide-based solid electrolyte other than the above-mentioned solid electrolytes.
[0047] The content of the solid electrolyte in the positive electrode mixture layer 24 is not particularly limited, but is preferably 1% by mass to 50% by mass, and more preferably 5% by mass to 30% by mass, based on the total mass of the positive electrode active material, the solid electrolyte, the conductive additive, and the binder.
[0048] The binder bonds the positive electrode active material, the solid electrolyte, and the conductive additive to one another within the positive electrode mixture layer 24, and also firmly bonds the positive electrode mixture layer 24 to the positive electrode current collector 22. The positive electrode mixture layer 24 preferably contains a binder. The binder preferably has oxidation resistance and good adhesiveness.
[0049] Examples of binders used in the positive electrode mixture layer 24 include polyvinylidene fluoride (PVDF) or its copolymers, polytetrafluoroethylene (PTFE), polyamide (PA), polyimide (PI), polyamideimide (PAI), polybenzimidazole (PBI), polyethersulfone (PES), polyacrylic acid (PA) and its copolymers, metal ion crosslinked polyacrylic acid (PA) and its copolymers, maleic anhydride-grafted polypropylene (PP), maleic anhydride-grafted polyethylene (PE), or mixtures thereof. Alternatively, a conductive polymer having electronic conductivity or an ionic conductive polymer having ionic conductivity may be used as the binder. Examples of conductive polymers having electronic conductivity include polyacetylene. In this case, the binder also functions as a conductive additive particle, so there is no need to add a conductive additive. As the ion-conductive polymer having ion conductivity, for example, a polymer that conducts lithium ions or the like can be used, and a monomer of a polymer compound (polyether polymer compounds such as polyethylene oxide and polypropylene oxide, polyphosphazene, etc.) and LiClO 4 , LiBF 4 , LiPF 6 Examples of the binder include a composite of the binder and a lithium salt such as LiTFSI or LiFSI, or an alkali metal salt mainly composed of lithium. The polymerization initiator used for the composite is, for example, a photopolymerization initiator or a thermal polymerization initiator that is compatible with the above-mentioned monomer. The properties required for the binder include oxidation / reduction resistance and good adhesiveness.
[0050] The binder content in the positive electrode mixture layer 24 is not particularly limited, but is preferably 1% by mass to 15% by mass, and more preferably 3% by mass to 5% by mass, based on the total mass of the positive electrode active material, solid electrolyte, conductive additive, and binder. If the binder content is too small, it tends to be difficult to form a positive electrode 20 with sufficient adhesive strength. Conversely, if the binder content is too high, general binders are electrochemically inactive and do not contribute to discharge capacity, making it difficult to obtain sufficient volume or mass energy density.
[0051] The conductive additive improves the electronic conductivity of the positive electrode mixture layer 24. Known conductive additives can be used. Examples of the conductive additive include carbon materials such as carbon black, graphite, carbon nanotubes, and graphene; metals such as aluminum, copper, nickel, stainless steel, iron, and amorphous metals; conductive oxides such as ITO; and mixtures thereof. The conductive additive may be in the form of powder or fiber.
[0052] There are no particular limitations on the content of the conductive additive in the positive electrode mixture layer 24. When a conductive additive is added, the mass ratio of the conductive additive is usually preferably 0.5% by mass to 20% by mass, and more preferably 1% by mass to 5% by mass, based on the total mass of the positive electrode active material, solid electrolyte, conductive additive, and binder.
[0053] 4, the negative electrode 30 has a negative electrode current collector 32 and a negative electrode mixture layer 34. The negative electrode mixture layer 34 is in contact with the negative electrode current collector 32.
[0054] The negative electrode current collector 32 may be any material as long as it has electronic conductivity. The negative electrode current collector 32 may be made of, for example, a metal such as copper, aluminum, nickel, stainless steel, or iron, an alloy thereof, or a conductive resin. The negative electrode current collector 32 may be in the form of a powder, a foil, a punched piece, or an expanded piece.
[0055] The negative electrode mixture layer 34 contains a negative electrode active material, and optionally a solid electrolyte, a binder, and a conductive additive.
[0056] The negative electrode active material is not particularly limited as long as it can reversibly absorb and release lithium ions and insert and extract lithium ions. As the negative electrode active material, any negative electrode active material used in known solid electrolyte batteries can be used.
[0057] Examples of the negative electrode active material include carbon materials such as natural graphite, artificial graphite, mesocarbon microbeads, mesocarbon fiber (MCF), cokes, glassy carbon, and organic compound sintered bodies, Si, SiO x Metals that can be combined with lithium, such as Sn and aluminum, alloys of these, composite materials of these metals and carbon materials, lithium titanate (Li4 Ti 5 O 12 ), SnO 2 The negative electrode active material is preferably natural graphite.
[0058] The solid electrolyte contained in the negative electrode 30 is, for example, the above-mentioned solid electrolyte. The solid electrolyte contained in the negative electrode 30 may be a halide-based solid electrolyte other than the above-mentioned solid electrolytes.
[0059] The binder and conductive additive contained in the negative electrode 30 may be the same as or different from the binder and conductive additive contained in the positive electrode 20 .
[0060] <Exterior Body> The exterior body 50 houses the power generating element 40 inside. The exterior body 50 prevents moisture and the like from entering from the outside to the inside. As shown in Fig. 4 , the exterior body 50 has a metal foil 52 and a resin layer 54 laminated on each side of the metal foil 52. The exterior body 50 is a metal laminate film in which the metal foil 52 is coated with the resin layer 54 from both sides.
[0061] The metal foil 52 is, for example, aluminum foil or stainless steel foil. The resin layer 54 can be, for example, a resin film such as polypropylene. The materials constituting the inner and outer resin layers 54 may be different. For example, the outer material can be a polymer with a high melting point, such as polyethylene terephthalate (PET) or polyamide (PA), and the inner material can be polyethylene (PE) or polypropylene (PP).
[0062] <Terminals> The terminals 60 and 62 are connected to the positive electrode 20 and the negative electrode 30, respectively. The terminal 60 connected to the positive electrode 20 is a positive electrode terminal, and the terminal 62 connected to the negative electrode 30 is a negative electrode terminal. The terminals 60 and 62 are responsible for electrical connection to the outside. The terminals 60 and 62 are made of a conductive material such as aluminum, nickel, or copper. The connection method may be welding or screw fastening. It is preferable to protect the terminals 60 and 62 with insulating tape to prevent short circuits.
[0063] "Method for manufacturing a solid electrolyte" Next, a method for manufacturing a solid electrolyte battery according to this embodiment will be described. A method for manufacturing a solid electrolyte represented by formula (1) will be described. The solid electrolyte can be obtained by mixing and reacting raw material powders in a predetermined molar ratio to obtain a desired composition. There is no particular restriction on the reaction method, and mechanochemical milling, sintering, melting, liquid phase method, solid phase method, etc. can be used.
[0064] Solid electrolytes can be manufactured, for example, by mechanochemical milling. First, a planetary ball mill is prepared. A planetary ball mill is a device in which media (hard balls used to promote grinding or mechanochemical reactions) and materials are placed in a dedicated container, and the mill rotates and revolves to grind the materials or induce mechanochemical reactions between the materials.
[0065] The solid electrolyte is prepared by preparing a predetermined amount of zirconia balls in a zirconia container in a glove box in which argon gas is circulated, for example. From the viewpoint of stably synthesizing the target compound, the dew point in the glove box is preferably −30° C. or lower and −90° C. or higher.
[0066] Next, predetermined raw materials are prepared in a zirconia container in a predetermined molar ratio to obtain the desired composition, and the container is sealed with a zirconia lid. The raw materials may be powder or liquid. Next, mechanochemical milling is performed for a predetermined time at predetermined rotation and revolution speeds, causing a mechanochemical reaction. This method allows for the production of a powdered solid electrolyte composed of compounds having the desired composition. As long as such synthesis is possible, there are no limitations on the preparation method, and heating and cooling may be performed during synthesis.
[0067] When a halide raw material is contained in the raw powder, the halide raw material is likely to evaporate when the temperature is increased. Therefore, halogen gas may be present in the sintering atmosphere to compensate for the halogen. Furthermore, when a halide raw material is contained in the raw powder, sintering may be performed by hot pressing using a mold with high airtightness. In this case, the mold has high airtightness, so evaporation of the halide raw material due to sintering can be suppressed. By sintering in this manner, a solid electrolyte in the form of a sintered body made of a compound having a predetermined composition is obtained.
[0068] "Preparation of a mixture for a positive electrode mixture layer" A mixture for a positive electrode mixture layer is prepared by mixing a positive electrode active material and a conductive additive. Any method can be used as long as it can be mixed uniformly, but dry mixing, wet mixing, etc. can be used. A binder and the above-mentioned solid electrolyte may also be mixed into the above-mentioned mixture for a positive electrode.
[0069] "Preparation of Mixture for Negative Electrode Mixture Layer" A mixture for a negative electrode mixture layer is prepared by mixing a negative electrode active material and a conductive additive. Any method can be used as long as it can be mixed uniformly, but dry mixing, wet mixing, etc. can be used. A binder and the above-mentioned solid electrolyte may also be mixed into the above-mentioned mixture for a negative electrode.
[0070] "Method for manufacturing the power generating element" Next, a method for manufacturing the power generating element 40 according to this embodiment will be described. The power generating element 40 according to this embodiment is manufactured using, for example, a powder molding method. The powder molding method is performed in an environment where the dew point is lower than -20°C and higher than -90°C. For example, the powder molding method is performed by adjusting the dew point inside a glove box.
[0071] First, a resin holder having a through hole in the center, a lower punch, and an upper punch are prepared. To improve formability, a metal holder made of die steel may be used instead of the resin holder. The diameter of the through hole in the resin holder is, for example, 10 mm, and the diameters of the lower punch and upper punch are, for example, 9.99 mm. The lower punch is inserted from below the through hole in the resin holder, and powdered solid electrolyte is poured from the opening side of the resin holder. Next, the upper punch is inserted on top of the poured powdered solid electrolyte, and the resin holder is placed in a press and pressed. The pressing pressure is, for example, 373 MPa. The powdered solid electrolyte is pressed between the upper punch and the lower punch within the resin holder to form the solid electrolyte layer 10.
[0072] Next, the upper punch is temporarily removed, and a mixture for a positive electrode active material layer is placed on the upper punch side of the solid electrolyte layer 10. Thereafter, the upper punch is reinserted, and pressing is performed. The pressing pressure is, for example, 373 MPa. The positive electrode mixture layer 24 is formed by pressing.
[0073] Next, the lower punch is temporarily removed, and the anode active material layer mixture is placed on the lower punch side of the solid electrolyte layer 10. For example, the sample is turned upside down, and the anode active material layer mixture is placed on top of the solid electrolyte layer 10 so that it faces the cathode active material layer 24. Thereafter, the lower punch is inserted again, and pressing is performed. The pressing pressure is, for example, 373 MPa. The anode active material layer mixture becomes the anode active material layer 34 by pressing.
[0074] Next, the upper punch is temporarily removed, and the positive electrode current collector 22 and the upper punch are inserted in this order onto the positive electrode active material layer 24. The lower punch is also temporarily removed, and the negative electrode current collector 32 and the lower punch are inserted in this order onto the negative electrode active material layer 34. The positive electrode current collector 22 and the negative electrode current collector 32 are, for example, aluminum foil or copper foil with a diameter of 10 mm. Through the above procedure, the power generating element 40 of this embodiment, consisting of the positive electrode current collector 22 / positive electrode active material layer 24 / solid electrolyte layer 10 / negative electrode active material layer 34 / negative electrode current collector 32, is obtained.
[0075] If necessary, the power generating element 40 may be a stainless steel disk or a Bakelite disk having four screw holes, stacked in the following order: stainless steel disk / Bakelite disk / upper punch / power generating element 40 / lower punch / Bakelite disk / stainless steel disk, and then fastened with the four screws. This is preferable from the viewpoint of further improving the bonding between the upper punch and the positive electrode current collector 22, the positive electrode current collector 22 and the positive electrode active material 24, the lower punch and the negative electrode current collector 32, and the negative electrode current collector 32 and the negative electrode active material 34. The power generating element 40 may have a similar mechanism having such a shape-retaining function.
[0076] - Storage Step - The storage step is performed, for example, in a glove box in which argon gas is circulated. The dew point in the glove box is lower than -20°C and higher than -90°C. The dew point in the glove box is preferably lower than -30°C and higher than -85°C.
[0077] Screws are inserted into the screw holes provided on the side surfaces of the upper punch and the lower punch, and the punch is inserted into the exterior body to which the external terminals are attached. The screws attached to the side surfaces of the upper punch and the lower punch are connected to the external terminals with lead wires or the like. The punch is then housed in the exterior body 50, and the opening of the exterior body 50 is heat-sealed to seal it. The solid electrolyte battery of this embodiment is obtained by the above process.
[0078] The solid electrolyte battery 100 according to this embodiment includes the above-described solid electrolyte, and therefore forms a conduction path that is less likely to bind lithium ions, and locally non-uniform electrochemical reactions are suppressed, thereby improving the rate characteristics of the solid electrolyte battery.
[0079] The above describes the embodiments of the present invention in detail with reference to the drawings. However, each configuration and combination thereof in each embodiment is an example, and additions, omissions, substitutions, and other modifications of the configurations are possible within the scope that does not deviate from the spirit of the present invention.
[0080] "Example 1" (Preparation of solid electrolyte) In a glove box with a dew point of about -75°C, zirconium chloride (ZrCl 4 ) and lithium sulfate (Li 2 SO 4) were weighed out to a molar ratio of 1:1, and the raw material powders were placed in a zirconia sealed container for a planetary ball mill that had previously contained zirconia balls and was dried under the same conditions. Next, a lid was placed on the sealed container, the lid was screwed onto the container body, and the gap between the lid and the sealed container was further sealed with polyimide tape. The zirconia balls, the zirconia sealed container for the planetary ball mill, and the lid were dried under reduced pressure at 80°C and returned to room temperature before use. Ar gas (G1 grade, manufactured by Taiyo Nippon Sanso Corporation) was used to return the pressure to atmospheric pressure. The polyimide tape has the effect of blocking moisture. Next, the zirconia sealed container was set in a planetary ball mill and subjected to a mechanochemical reaction for 5 hours at a rotation speed of 300 rpm to obtain a solid electrolyte (Li 2 Zr(SO 4 ) Cl 4 The ratio of rotation to revolution was 1:1. The synthesis was started after cooling the zirconia sealed container and lid to a temperature of 10°C or less, and the synthesis was continued while cooling.
[0081] The planetary ball mill was installed in a normal atmosphere (air). The zirconia airtight container for the planetary ball mill was screwed in and sealed with polyimide tape. When the zirconia airtight container was set in the planetary ball mill, the zirconia airtight container was firmly pressed in place from the lid, preventing the lid from being released. Therefore, even in a normal atmosphere, it is believed that almost no moisture from the air gets into the zirconia airtight container.
[0082] <Measurement of Raman Spectrum> The Raman spectrum of the solid electrolyte of Example 1 was measured by Raman spectroscopy. Sampling was carried out in a glove box with circulating argon gas at a dew point of approximately -70°C, and the sample was transported to a Raman spectrometer (manufactured by JASCO Corporation: NRS-7100) without being exposed to the atmosphere, and measurement was carried out. The Raman spectrum was measured under the following conditions: laser wavelength: 532 nm, slit width: 100 × 1000 μm, aperture: 40 μm, exposure time: 60 sec, and integration: 2 times. The 900-1250 cm of the obtained Raman spectrum -1 In the range 950 to 1025 cm -1Peak a having a peak top in the range 1026 to 1110 cm -1 The peak b having a peak top at 900-1250 cm of the obtained Raman spectrum was confirmed. -1 The line connecting these peaks was used as the baseline, and the intensities Ia and Ib of each peak were measured. The measured Raman spectrum of Example 1 is shown in FIG.
[0083] <XPS Measurement> X-ray photoelectron spectroscopy measurement was also performed on the solid electrolyte of Example 1. Sampling was performed in a glove box with circulating argon gas at a dew point of approximately -70°C, and the sample was transported to an XPS measurement device without being exposed to the atmosphere. The XPS measurement was performed using a Quantera 2 manufactured by PHI Corporation. As a result, peaks were confirmed at 170±0.5 eV and 532±0.5 eV for the produced solid electrolyte.
[0084] -Mixing of Positive Electrode Mixture- Next, the positive electrode mix was weighed and mixed in a glove box with argon gas circulating at a dew point of -75°C. 2 ): Li 2 Zr(SO 4 ) Cl 4 The mixture was weighed to a ratio of 75:19:6 parts by weight of lithium cobalt oxide and carbon black, and mixed in an agate mortar for 5 minutes to obtain a positive electrode mixture. The agate mortar, lithium cobalt oxide, and carbon black used in the mixing were dried under reduced pressure as in the zirconia sealed container before use. The lithium cobalt oxide used had an average particle size of 7.5 μm.
[0085] - Preparation of negative electrode mixture - Next, the negative electrode mixture was weighed and mixed in a glove box with argon gas circulating therein and a dew point of -75°C. 4 Ti 5 O 12 ): Li 2 Zr(SO 4 ) Cl 4The mixture was weighed to a ratio of 72:22:6 parts by weight of lithium titanate and carbon black, and mixed in an agate mortar for 5 minutes to obtain a negative electrode mixture. The agate mortar, lithium titanate, and carbon black used for mixing were dried under reduced pressure as in the zirconia sealed container before use. The lithium titanate used had an average particle size of 6.0 μm.
[0086] (Fabrication of Solid Electrolyte Battery) The solid electrolyte battery was fabricated in a glove box with a dew point of approximately -75°C. The solid electrolyte battery was fabricated using a pellet fabrication jig. The pellet fabrication jig had a PEEK (polyether ether ketone) holder with an inner diameter of 10 mm, and upper and lower punches with diameters of 9.99 mm. The upper and lower punches were made of die steel (SKD11 material).
[0087] A lower punch was inserted into a PEEK holder of a pellet-making jig, and 50 mg of solid electrolyte was placed on the lower punch. The resin holder was then vibrated to smooth the surface of the solid electrolyte, after which an upper punch was inserted onto the solid electrolyte and pressed with a press under a load of approximately 4 kN.
[0088] Next, the lower punch was removed, and 10 mg of a negative electrode mixture was placed on the solid electrolyte. Next, the PEEK holder was vibrated to level the surface of the negative electrode mixture, and then the lower punch was inserted onto the negative electrode mixture and pressed with a press under a load of 3 KN.
[0089] Next, the upper punch was removed, and 12 mg of a positive electrode mixture was placed on the solid electrolyte layer. The PEEK holder was then vibrated to level the surface of the positive electrode mixture, after which the upper punch was inserted onto the positive electrode mixture and pressed with a press under a load of 3 KN.
[0090] Next, the upper punch was removed, and a positive electrode current collector (aluminum foil, 10 mm in diameter, 20 μm in thickness) and the upper punch were inserted in this order onto the positive electrode mixture layer. The lower punch was also removed, and a negative electrode current collector (copper foil, 10 mm in diameter, 10 μm in thickness) and the lower punch were inserted in this order onto the negative electrode mixture layer. In this way, a power generation element consisting of a positive electrode current collector / positive electrode mixture layer / solid electrolyte layer / negative electrode mixture layer / negative electrode current collector was produced.
[0091] A 50 mm diameter, 5 mm thick stainless steel disk and a Bakelite (registered trademark) disk with four screw holes were prepared, and the power generation element was set as follows: Stainless steel disk / Bakelite disk / upper punch / power generation element / lower punch / Bakelite disk / stainless steel disk were stacked in this order, and the four screws were tightened with a torque of 1 N m to create a power generation element unit. Screws for connecting external terminals were inserted into the screw holes on the side of the upper punch and lower punch.
[0092] Next, an A4-sized aluminum laminate bag was prepared as an exterior body to enclose the power generation element unit. Aluminum foil (4 mm wide, 40 mm long, 100 μm thick) wrapped with maleic anhydride-grafted polypropylene (PP) and nickel foil (4 mm wide, 40 mm long, 100 μm thick) were thermally bonded to one side of the opening of the aluminum laminate bag at a distance to prevent short-circuiting. The power generation element unit was inserted into the aluminum laminate bag with the attached external terminals, and lead wires were connected between the screw on the side of the upper punch and the aluminum terminal extending inside the exterior body, and between the screw on the side of the lower punch and the nickel terminal extending inside the exterior body. Finally, the opening was heat-sealed to produce a solid electrolyte battery. The fabricated solid electrolyte battery was placed in a constant temperature bath at 25°C for 48 hours to stabilize the open-circuit voltage.
[0093] The rate characteristics were evaluated using the prepared solid electrolyte battery. The rate characteristics were evaluated from the ratio (Cap0.5C / Cap0.1C) of the discharge capacity (Cap1C) when discharged at a discharge rate of 0.5C to the charge capacity (Cap0.1C). The solid electrolyte battery was placed in a 25°C environment and subjected to constant current charging (CC charging) at a constant current of 0.1C rate until the battery voltage reached 2.7V. After reaching 2.7V, the battery was charged to a current equivalent to 0.05C (CV charging), and the charge capacity at 0.1C (Cap0.1C) was measured. Then, the battery was discharged at a constant current of 0.5C rate until the battery voltage reached 1.5V (CC discharge), and the discharge capacity at 0.5C (Cap0.5C) was measured. The measurement results are summarized in Tables 3 and 4.
[0094] Example 2 In Example 2, a solid electrolyte was synthesized in the same manner as in Example 1, except that the synthesis time was changed, and Raman analysis and rate characteristic evaluation were performed. The measured Raman spectrum is shown in Figure 2. The measurement results are also summarized in Tables 3 and 4.
[0095] In Examples 3 to 30, solid electrolytes were synthesized in the same manner as in Example 1, except that the raw materials and / or molar ratios and the synthesis time were changed, and Raman analysis and rate characteristic evaluation were performed. The results are summarized in Tables 1, 2, 3, and 4.
[0096] Example 31 In Example 31, a solid electrolyte was synthesized in the same manner as in Example 1 except for changing the synthesis time, and Raman analysis and rate characteristic evaluation were performed. The results are summarized in Tables 5 and 6.
[0097] Comparative Example 1 In Comparative Example 1, a solid electrolyte was synthesized in the same manner as in Example 1 except that the synthesis time was changed, and Raman analysis and rate characteristic evaluation were performed. The measured Raman spectrum is shown in Figure 3. The measurement results are summarized in Tables 3 and 4.
[0098] In Comparative Examples 1 to 15, solid electrolytes were synthesized in the same manner as in Example 1, except that the raw materials and / or molar ratios and the synthesis time were changed, and Raman analysis and rate characteristic evaluation were performed. The results are summarized in Tables 1, 2, 3, and 4.
[0099] Comparative Example 16 In Comparative Example 16, a solid electrolyte was synthesized in the same manner as in Example 31, except that cooling was not performed, and Raman analysis and rate characteristic evaluation were performed. The results are summarized in Tables 5 and 6.
[0100]
[0101]
[0102]
[0103]
[0104]
[0105]
[0106] Example 1, Example 2, and Comparative Example 1 have the same composition, but the synthesis times are different. Accordingly, in the Raman spectra, the appearance of peaks a and b was confirmed in Examples 1 and 2, but peak b was not confirmed in Comparative Example 1. Differences were also confirmed in peak intensity Ia and peak intensity Ib, with Ia > Ib in Example 1 and Ia < Ib in Example 2. The rate characteristics of each were best in Example 1, followed by Example 2 and finally Comparative Example 1. As described above, even with the same composition, the rate characteristics could be improved by adjusting the Raman spectrum to a predetermined value.
[0107] Example 3, Example 4, and Comparative Example 2 have the same composition, but the synthesis times are different. Accordingly, in the Raman spectra, the appearance of peaks a and b was confirmed in Examples 3 and 4, but peak b was not confirmed in Comparative Example 2. Differences were also confirmed in peak intensity Ia and peak intensity Ib, with Ia > Ib in Example 3 and Ia < Ib in Example 4. The rate characteristics of each were best in Example 3, followed by Example 4 and finally Comparative Example 2. As described above, even with the same composition, the rate characteristics could be improved by adjusting the Raman spectrum to a predetermined value.
[0108] Example 5, Example 6, and Comparative Example 3 have the same composition, but the synthesis times are different. Accordingly, in the Raman spectra, the appearance of peaks a and b was confirmed in Examples 5 and 6, but peak b was not confirmed in Comparative Example 3. Differences were also confirmed in peak intensity Ia and peak intensity Ib, with Ia > Ib in Example 5 and Ia < Ib in Example 6. The rate characteristics of each were best in Example 5, followed by Example 6 and finally Comparative Example 3. As described above, even with the same composition, the rate characteristics could be improved by adjusting the Raman spectrum to a predetermined value.
[0109] Example 7, Example 8, and Comparative Example 4 have the same composition, but the synthesis times are different. Accordingly, in the Raman spectra, the appearance of peaks a and b was confirmed in Examples 7 and 8, but peak b was not confirmed in Comparative Example 4. Differences were also confirmed in peak intensity Ia and peak intensity Ib, with Ia > Ib in Example 7 and Ia < Ib in Example 8. The rate characteristics of each were best in Example 7, followed by Example 8 and finally Comparative Example 4. As described above, even with the same composition, the rate characteristics could be improved by adjusting the Raman spectrum to a predetermined value.
[0110] Example 9, Example 10, and Comparative Example 5 have the same composition, but the synthesis time is different. Accordingly, in the Raman spectrum, the appearance of peaks a and b was confirmed in Examples 9 and 10, but peak b was not confirmed in Comparative Example 5. Differences were also confirmed in peak intensity Ia and peak intensity Ib, with Ia > Ib in Example 9 and Ia < Ib in Example 10. The rate characteristics of each were the best in Example 9, followed by Example 10 and finally Comparative Example 5. As described above, even with the same composition, the rate characteristics could be improved by adjusting to obtain a predetermined Raman spectrum.
[0111] Example 11, Example 12, and Comparative Example 6 have the same composition, but the synthesis times are different. Accordingly, in the Raman spectra, the appearance of peaks a and b was confirmed in Examples 11 and 12, but peak b was not confirmed in Comparative Example 6. Differences were also confirmed in peak intensity Ia and peak intensity Ib, with Ia > Ib in Example 11 and Ia < Ib in Example 12. The rate characteristics of each were best in Example 11, followed by Example 12 and finally Comparative Example 6. As described above, even with the same composition, the rate characteristics could be improved by adjusting the Raman spectrum to a predetermined value.
[0112] Examples 13, 14, and Comparative Example 7 have the same composition, but the synthesis times are different. Accordingly, in the Raman spectra, the appearance of peaks a and b was confirmed in Examples 13 and 14, but peak b was not confirmed in Comparative Example 7. Differences were also confirmed in peak intensity Ia and peak intensity Ib, with Ia > Ib in Example 13 and Ia < Ib in Example 14. The rate characteristics of each were best in Example 13, followed by Example 14 and finally Comparative Example 7. As described above, even with the same composition, the rate characteristics could be improved by adjusting the Raman spectrum to a predetermined value.
[0113] Example 15, Example 16, and Comparative Example 8 have the same composition, but the synthesis time is different. Accordingly, in the Raman spectrum, the appearance of peaks a and b was confirmed in Examples 15 and 16, but peak b was not confirmed in Comparative Example 8. Differences were also confirmed in peak intensity Ia and peak intensity Ib, with Ia > Ib in Example 15 and Ia < Ib in Example 16. The rate characteristics of each were the best in Example 15, followed by Example 16 and finally Comparative Example 8. As described above, even with the same composition, the rate characteristics could be improved by adjusting to obtain a predetermined Raman spectrum.
[0114] Example 17, Example 18, and Comparative Example 9 have the same composition, but the synthesis times are different. Accordingly, in the Raman spectra, the appearance of peaks a and b was confirmed in Examples 17 and 18, but peak b was not confirmed in Comparative Example 9. Differences were also confirmed in peak intensity Ia and peak intensity Ib, with Ia > Ib in Example 17 and Ia < Ib in Example 18. The rate characteristics of each were best in Example 17, followed by Example 18 and finally Comparative Example 9. As described above, even with the same composition, the rate characteristics could be improved by adjusting the Raman spectrum to a predetermined value.
[0115] Example 19, Example 20, and Comparative Example 10 have the same composition, but different synthesis times. Accordingly, in the Raman spectra, the appearance of peaks a and b was confirmed in Examples 19 and 20, but peak b was not confirmed in Comparative Example 10. Differences were also confirmed in peak intensity Ia and peak intensity Ib, with Ia > Ib in Example 19 and Ia < Ib in Example 20. The rate characteristics of each were the best in Example 19, followed by Example 20 and finally Comparative Example 10. As described above, even with the same composition, the rate characteristics could be improved by adjusting to obtain a predetermined Raman spectrum.
[0116] Example 21, Example 22, and Comparative Example 11 have the same composition, but different synthesis times. Accordingly, in the Raman spectra, the appearance of peaks a and b was confirmed in Examples 21 and 22, but peak b was not confirmed in Comparative Example 11. Differences were also confirmed in peak intensity Ia and peak intensity Ib, with Ia > Ib in Example 21 and Ia < Ib in Example 22. The rate characteristics of each were best in Example 21, followed by Example 22 and finally Comparative Example 11. As described above, even with the same composition, the rate characteristics could be improved by adjusting the Raman spectrum to a predetermined value.
[0117] Examples 23, 24, and Comparative Example 12 have the same composition, but different synthesis times. Accordingly, in the Raman spectra, the appearance of peaks a and b was confirmed in Examples 23 and 24, but peak b was not confirmed in Comparative Example 12. Differences were also confirmed in peak intensity Ia and peak intensity Ib, with Ia > Ib in Example 23 and Ia < Ib in Example 24. The rate characteristics of each were the best in Example 23, followed by Example 24 and finally Comparative Example 12. As described above, even with the same composition, the rate characteristics could be improved by adjusting the Raman spectrum to a predetermined value.
[0118] Example 25, Example 26, and Comparative Example 13 have the same composition, but the synthesis time is different. Accordingly, in the Raman spectrum, the appearance of peaks a and b was confirmed in Examples 25 and 26, but peak b was not confirmed in Comparative Example 13. Differences were also confirmed in peak intensity Ia and peak intensity Ib, with Ia > Ib in Example 25 and Ia < Ib in Example 26. The rate characteristics of each were the best in Example 25, followed by Example 26 and finally Comparative Example 13. As described above, even with the same composition, the rate characteristics could be improved by adjusting to obtain a predetermined Raman spectrum.
[0119] Example 27, Example 28, and Comparative Example 14 have the same composition, but different synthesis times. Accordingly, in the Raman spectra, the appearance of peaks a and b was confirmed in Examples 27 and 28, but peak b was not confirmed in Comparative Example 14. Differences were also confirmed in peak intensity Ia and peak intensity Ib, with Ia > Ib in Example 27 and Ia < Ib in Example 28. The rate characteristics of each were best in Example 27, followed by Example 28 and finally Comparative Example 14. As described above, even with the same composition, the rate characteristics could be improved by adjusting the Raman spectrum to a predetermined value.
[0120] Example 29, Example 30, and Comparative Example 15 have the same composition, but different synthesis times. Accordingly, in the Raman spectra, the appearance of peaks a and b was confirmed in Examples 29 and 30, but peak b was not confirmed in Comparative Example 15. Differences were also confirmed in peak intensity Ia and peak intensity Ib, with Ia > Ib in Example 29 and Ia < Ib in Example 30. The rate characteristics of each were the best in Example 29, followed by Example 30 and finally Comparative Example 15. As described above, even with the same composition, the rate characteristics could be improved by adjusting the Raman spectrum to a predetermined value.
[0121] Example 1, Example 2, Example 31, and Comparative Example 1 have the same composition, but the synthesis times are different. Accordingly, in the Raman spectra, the appearance of peaks a and b was confirmed in Examples 1, 2, and 31, but peak b was not confirmed in Comparative Example 1. Differences were also confirmed in peak intensity Ia and peak intensity Ib, with Ia > Ib in Examples 1 and 31 and Ia < Ib in Example 2. The rate characteristics of each were best in Example 1, followed by Example 31, then Example 2, and finally Comparative Example 1. As described above, even with the same composition, the rate characteristics could be improved by adjusting the Raman spectrum to a predetermined value.
[0122] Example 31 and Comparative Example 16 had the same composition and synthesis time, but differed in whether or not cooling was performed during synthesis. Accordingly, in the Raman spectrum, the appearance of peaks a and b was confirmed in Example 31, and the peak intensities Ia and Ib were Ia > Ib. In Comparative Example 16, peak a was not clearly confirmed, but when the intensity of the Raman spectrum in the vicinity was assumed to be Ia, Ia < Ib was obtained. The rate characteristics of Example 31 were better than those of Comparative Example 16. As described above, even with the same composition, the rate characteristics could be improved by adjusting the Raman spectrum to a predetermined value.
[0123] It is possible to provide a solid electrolyte capable of improving rate characteristics, a solid electrolyte layer using the same, and a solid electrolyte battery.
[0124] REFERENCE SIGNS LIST 10... solid electrolyte layer, 20... positive electrode, 22... positive electrode current collector, 24... positive electrode mixture layer, 30... negative electrode, 32... negative electrode current collector, 34... negative electrode mixture layer, 40... power generating element, 50... exterior body, 52... metal foil, 54... resin layer, 60, 62... terminal, 100... solid electrolyte battery
Claims
1. The Raman spectrum of the compound represented by formula (1) measured at an excitation wavelength of 532 nm is 900-1250 cm -1 In the range 950 to 1025 cm -1 Peak a with a peak top in the range 1026-1110 cm -1 A solid electrolyte having two or more peaks, i.e., a peak b having a peak top at Li a A b Zr c B d (SO 4 ) e C f X g ... (1) (In the formula, A is at least one element selected from alkali metals and alkaline earth metals, B is at least one element selected from the group consisting of Na, K, Rb, Cs, Mg, Ca, Sr, Ba, B, Si, Al, Ti, Cu, Sc, Y, Zr, Nb, Ag, In, Sn, Sb, Hf, Ta, W, Au, and Bi, and X is at least one element selected from the group consisting of F, Br, and I, and 0.5≦a<6, 0≦b<6, 0<c<2, 0≦d<1, 0<e<3, 0<f≦5, and 0≦g<5.) 2. Raman spectrum 900-1250 cm -1 2. The solid electrolyte according to claim 1, wherein when the intensities of peak a and peak b are Ia and Ib, respectively, relative to a straight line connecting the above lines and a baseline, Ia>Ib.
3. A solid electrolyte layer comprising the solid electrolyte according to claim 1 or 2.
4. A solid electrolyte battery comprising a solid electrolyte layer, a positive electrode, and a negative electrode, at least one of the positive electrode and the negative electrode containing the solid electrolyte according to claim 1 or 2.
5. A solid electrolyte battery comprising the solid electrolyte layer according to claim 3, a positive electrode and a negative electrode.
Citation Information
Patent Citations
Solid electrolyte and solid electrolyte battery
WO2021261558A1
Lithium-based solid electrolyte, inorganic solid electrolyte, lithium-based solid electrolyte production method, modified positive electrode active material, modified negative electrode active material, all-solid-state secondary battery, electrode sheet for all-solid-state secondary battery, solid electrolyte sheet, electrode for all-solid-state secondary battery
WO2022118870A2
Cited By
Negative electrode layer and solid state battery
WO2026196761A1