Thermoplastic liquid crystal polymer film and laminate
By optimizing the surface roughness of thermoplastic liquid crystal polymer films, specifically the maximum valley depth, the adhesion of conductive ink is enhanced, addressing the issue of ink bleeding and enabling the creation of fine circuits with improved adhesion and conductivity.
Patent Information
- Application Number
- PCT/JP2024/012020
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-03
AI Technical Summary
Thermoplastic liquid crystal polymer films exhibit poor adhesion of conductive ink due to low hygroscopicity, leading to issues with ink bleeding and poor fine pattern formation, despite their excellent heat resistance and flexibility.
Adjusting the surface roughness parameters of the thermoplastic liquid crystal polymer films, specifically the maximum valley depth (Sv) to a predetermined range, enhances ink adhesion without increasing wettability, allowing for fine circuit processing and preventing ink bleeding.
The adjusted surface roughness improves conductive ink adhesion and prevents ink bleeding, enabling the formation of fine circuits with enhanced adhesion and conductivity on thermoplastic liquid crystal polymer films.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Thermoplastic liquid crystal polymer films and laminates Related Applications
[0001] This application claims priority to Japanese Patent Application No. 2023-053938, filed March 29, 2023, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a thermoplastic liquid crystal polymer film containing a polymer capable of forming an optically anisotropic melt phase (hereinafter referred to as a thermoplastic liquid crystal polymer), and a laminate containing a thermoplastic liquid crystal polymer film and a conductive layer laminated on at least one surface of the thermoplastic liquid crystal polymer film.
[0003] In recent years, printed electronics technology has attracted attention as a method for easily fabricating complex circuits. This technology uses conductive ink containing conductive particles such as silver nanoparticles or copper nanoparticles to form circuit patterns on a substrate by drawing or printing, and then firing the ink as needed to form conductive circuits on the substrate. In this process, the substrate must be heat-resistant enough to withstand firing. Glass and ceramic substrates are materials with excellent heat resistance, but it is difficult to make them thin in order to avoid brittle fracture.
[0004] In recent years, the use of flexible circuit boards using resins that have excellent toughness and can be formed into thin films as circuit substrates has been promoted. Patent Document 1 focuses on the excellent heat resistance of thermoplastic liquid crystal polymer films and describes a method for producing a conductive circuit board, in which a pattern is drawn on the surface of a substrate made of a thermotropic liquid crystal polymer film using ink containing metal fine particles, and the substrate is heated to sinter the metal fine particles and form a conductor pattern.
[0005] JP 2009-283667 A
[0006] Patent Document 1 points out that substrates made of thermoplastic liquid crystal polymers are resistant to thermal degradation and thermal deformation even during the sintering process of metal microparticles, and are less susceptible to brittle fracture even when thinned, resulting in excellent workability. On the other hand, thermoplastic liquid crystal polymer films have low hygroscopicity, resulting in poor adhesion of conductive ink. To solve this problem, Patent Document 1 proposes adjusting the surface free energy by physical treatments such as ultraviolet irradiation, corona discharge, and plasma treatment, or chemical treatment. However, if these treatments increase the wettability of the conductive ink too much, the ink will bleed on the substrate surface, making it difficult to form fine patterns.
[0007] The present invention aims to provide a thermoplastic liquid crystal polymer film that can be used to process fine circuits using conductive ink and has excellent adhesion to the formed circuits, and a laminate comprising such a thermoplastic liquid crystal polymer film and a conductive layer.
[0008] As a result of intensive research to achieve the above-mentioned object, the inventors of the present invention focused on parameters that indicate the surface shape of a thermoplastic liquid crystal polymer film, and discovered that by adjusting the maximum valley depth Sv of the film surface within a predetermined range, it is possible to improve the adhesion of conductive ink to the film without improving the wettability of the film surface by treatments such as ultraviolet irradiation or plasma irradiation, thereby avoiding ink bleeding and enabling fine circuit processing, and thus completed the present invention.
[0009] That is, the present invention can be configured in the following aspects. [Aspect 1] A thermoplastic liquid crystal polymer film containing a polymer capable of forming an optically anisotropic melt phase (hereinafter referred to as a thermoplastic liquid crystal polymer), wherein the maximum valley depth Sv on at least one surface is 0.15 μm or more (preferably 0.2 μm or more, more preferably greater than 0.40 μm, and even more preferably 0.5 μm or more) and 2.0 μm or less (preferably 1.5 μm or less, more preferably 1.0 μm or less). [Aspect 2] The thermoplastic liquid crystal polymer film according to Aspect 1, wherein the maximum height Sz of the front surface is 2.5 μm or less (preferably 2.0 μm or less). [Aspect 3] The thermoplastic liquid crystal polymer film according to Aspect 1 or 2, wherein the ratio Sv / Sz of the maximum valley depth Sv to the maximum height Sz of the surface is 0.6 or more (preferably 0.7 or more) and 1 or less. [Aspect 4] The thermoplastic liquid crystal polymer film according to any one of Aspects 1 to 3, wherein the surface protrusion height Spk is 0.03 μm or more (preferably 0.10 μm or more, more preferably greater than 0.10 μm, for example 0.11 μm or more) and 0.40 μm or less (preferably 0.25 μm or less, more preferably 0.2 μm or less). [Aspect 5] The thermoplastic liquid crystal polymer film according to any one of Aspects 1 to 4, wherein the melting point is 315° C. or more.
[0010] [Aspect 6] A laminate comprising a conductive layer laminated on at least one surface of the thermoplastic liquid crystal polymer film according to any one of Aspects 1 to 5. [Aspect 7] The laminate according to Aspect 6, wherein a layer composed of at least one material selected from the group consisting of conductive ink, metal film, and circuits formed therefrom is formed as a conductive layer on the surface of the thermoplastic liquid crystal polymer film. [Aspect 8] The laminate according to Aspect 6 or 7, wherein a metal foil layer is formed as a conductive layer on the surface opposite to the surface of the thermoplastic liquid crystal polymer film. [Aspect 9] The laminate according to any one of Aspects 6 to 8, wherein the laminate is a circuit board.
[0011] It should be noted that any combination of at least two elements disclosed in the claims and / or the specification is included in the present invention, and in particular any combination of two or more of the claims described in the claims is included in the present invention.
[0012] The thermoplastic liquid crystal polymer film of the present invention has a maximum valley depth adjusted to an appropriate range on at least one surface, so that the adhesion of conductive ink can be improved without any additional special physical or chemical treatment, and ink bleeding can be avoided, making it possible to form fine circuits.
[0013] (Thermoplastic liquid crystal polymer film) In the description of the present invention, the thermoplastic liquid crystal polymer film is a film containing a thermoplastic liquid crystal polymer.The thermoplastic liquid crystal polymer is composed of a liquid crystal polymer that can be melt-molded (or a polymer that can form an optically anisotropic melt phase), and as long as it is a liquid crystal polymer that can be melt-molded, its chemical structure is not particularly limited, but for example, it can be a thermoplastic liquid crystal polyester or a thermoplastic liquid crystal polyester amide that has an amide bond introduced therein.
[0014] The thermoplastic liquid crystal polymer may also be a polymer in which an isocyanate-derived bond such as an imide bond, a carbonate bond, a carbodiimide bond or an isocyanurate bond is further introduced into an aromatic polyester or an aromatic polyester amide.
[0015] Specific examples of the thermoplastic liquid crystal polymer used in the present invention include known thermoplastic liquid crystal polyesters and thermoplastic liquid crystal polyester amides derived from the compounds classified as (1) to (4) shown below and their derivatives. However, it goes without saying that there is an appropriate range for the combination of various raw material compounds in order to form a polymer that can form an optically anisotropic molten phase.
[0016] (1) Aromatic or aliphatic diol (see Table 1 for representative examples)
[0017] (2) Aromatic or aliphatic dicarboxylic acids (see Table 2 for representative examples)
[0018] (3) Aromatic hydroxycarboxylic acids (see Table 3 for representative examples)
[0019] (4) Aromatic diamines, aromatic hydroxyamines, or aromatic aminocarboxylic acids (see Table 4 for representative examples)
[0020] Representative examples of thermoplastic liquid crystal polymers obtained from these raw material compounds include copolymers having the repeating units shown in Tables 5 and 6.
[0021]
[0022] Among these copolymers, copolymers containing at least p-hydroxybenzoic acid and / or 6-hydroxy-2-naphthoic acid as repeating units are preferred, and particularly preferred are (i) copolymers containing repeating units of p-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid, or (ii) copolymers containing repeating units of at least one aromatic hydroxycarboxylic acid selected from the group consisting of p-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid, at least one aromatic diol and / or aromatic hydroxyamine, and at least one aromatic dicarboxylic acid.
[0023] For example, in the copolymer (i), when the thermoplastic liquid crystal polymer contains at least repeating units of p-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid, the molar ratio (A) / (B) of the p-hydroxybenzoic acid in the repeating unit (A) to the 6-hydroxy-2-naphthoic acid in the repeating unit (B) in the thermoplastic liquid crystal polymer is preferably about (A) / (B) = 10 / 90 to 90 / 10, more preferably about (A) / (B) = 15 / 85 to 85 / 15, and even more preferably about (A) / (B) = 20 / 80 to 80 / 20.
[0024] In the case of the copolymer (i), in addition to the repeating units of p-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid, from the viewpoint of adjusting the molecular weight, etc., it may contain repeating units composed of an aromatic diol or an aromatic dicarboxylic acid (for example, terephthalic acid).
[0025] In the case of the copolymer (ii), at least one aromatic hydroxycarboxylic acid (C) selected from the group consisting of p-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid, at least one aromatic diol (D) selected from the group consisting of 4,4'-dihydroxybiphenyl, hydroquinone, phenylhydroquinone, and 4,4'-dihydroxydiphenyl ether, and at least one aromatic dicarboxylic acid (E) selected from the group consisting of terephthalic acid, isophthalic acid, and 2,6-naphthalenedicarboxylic acid. The molar ratio of each repeating unit of the aromatic hydroxycarboxylic acid (C): the aromatic diol (D): the aromatic dicarboxylic acid (E) in the thermoplastic liquid crystal polymer may be about (30 to 80): (35 to 10): (35 to 10), more preferably about (C): (D): (E) = (35 to 75): (32.5 to 12.5): (32.5 to 12.5), and even more preferably about (C): (D): (E) = (40 to 70): (30 to 15): (30 to 15).
[0026] The molar ratio of repeating units derived from 6-hydroxy-2-naphthoic acid in the aromatic hydroxycarboxylic acid (C) may be, for example, 85 mol % or more, preferably 90 mol % or more, and more preferably 95 mol % or more. The molar ratio of repeating units derived from 2,6-naphthalenedicarboxylic acid in the aromatic dicarboxylic acid (E) may be, for example, 85 mol % or more, preferably 90 mol % or more, and more preferably 95 mol % or more.
[0027] Alternatively, the aromatic diol (D) may be repeating units (D1) and (D2) derived from two different aromatic diols selected from the group consisting of hydroquinone, 4,4'-dihydroxybiphenyl, phenylhydroquinone, and 4,4'-dihydroxydiphenyl ether. In this case, the molar ratio of the two aromatic diols (D1) / (D2) may be 23 / 77 to 77 / 23, more preferably 25 / 75 to 75 / 25, and even more preferably 30 / 70 to 70 / 30.
[0028] Furthermore, the molar ratio of the repeating structural units derived from the aromatic diol to the repeating structural units derived from the aromatic dicarboxylic acid, (D) / (E), is preferably 95 / 100 to 100 / 95. If the ratio is outside this range, the degree of polymerization does not increase and the mechanical strength tends to decrease.
[0029] The ability to form an optically anisotropic molten phase in the present invention can be confirmed, for example, by placing a sample on a hot stage, heating it in a nitrogen atmosphere, and observing the light transmitted through the sample.
[0030] Melting point of thermoplastic liquid crystal polymer (Tm 0) is preferably in the range of 300 to 380 ° C, more preferably in the range of 305 to 360 ° C, and even more preferably in the range of 310 to 350 ° C. The melting point of the thermoplastic liquid crystal polymer can be obtained by observing the thermal behavior of the thermoplastic liquid crystal polymer sample using a differential scanning calorimeter. That is, the thermoplastic liquid crystal polymer sample is heated at a rate of 10 ° C / min until it is completely melted, and then the melt is cooled to 50 ° C at a rate of 10 ° C / min, and the position of the endothermic peak that appears after heating again at a rate of 10 ° C / min is recorded as the melting point of the thermoplastic liquid crystal polymer sample.
[0031] Furthermore, from the viewpoint of melt moldability, the thermoplastic liquid crystal polymer is, for example, 0 The melt viscosity at a shear rate of 1000 / s at +20°C may be 30 to 120 Pa·s, and preferably 50 to 100 Pa·s.
[0032] The thermoplastic liquid crystal polymer film may contain a thermoplastic polymer such as polyethylene terephthalate, modified polyethylene terephthalate, polyolefin, polycarbonate, polyarylate, polyamide, polyphenylene sulfide, polyether ether ketone, or fluororesin, as well as various additives, within the scope of the present invention. Furthermore, it may contain a filler such as an organic filler or an inorganic filler, as necessary. Therefore, the thermoplastic liquid crystal polymer film of the present invention also includes a film made of a thermoplastic liquid crystal polymer composition containing a thermoplastic liquid crystal polymer as a main component and one or more of these heterogeneous polymers, additives, fillers, etc.
[0033] The thermoplastic liquid crystal polymer film may contain 50% by weight or more of thermoplastic liquid crystal polymer, preferably 80% by weight or more, more preferably 90% by weight or more, even more preferably 95% by weight or more, and even more preferably 98% by weight or more.
[0034] The thermoplastic liquid crystal polymer film may be a cast film of the above-mentioned thermoplastic liquid crystal polymer or thermoplastic liquid crystal polymer film composition, or may be an extrusion-molded film obtained by extruding a thermoplastic liquid crystal polymer or a thermoplastic liquid crystal polymer film composition. At this time, any extrusion molding method can be used, but the well-known T-die film stretching method, laminate stretching method, inflation method, etc. are industrially advantageous. In particular, in the inflation method, stress is applied not only in the machine axis direction (hereinafter abbreviated as MD direction) of the thermoplastic liquid crystal polymer film, but also in the direction perpendicular thereto (hereinafter abbreviated as TD direction), and it can be uniformly stretched in the MD direction and the TD direction, so that a thermoplastic liquid crystal polymer film with controlled molecular orientation, dielectric properties, etc. can be obtained.
[0035] In addition, the thermoplastic liquid crystal polymer film may be stretched as needed after extrusion molding.The stretching method itself is known, and either biaxial stretching or uniaxial stretching may be adopted, but biaxial stretching is preferred because it is easier to control the molecular orientation degree.In addition, for stretching, known uniaxial stretching machines, simultaneous biaxial stretching machines, sequential biaxial stretching machines, etc. can be used.
[0036] In extrusion molding, a stretching process may be performed to control the orientation. For example, in extrusion molding using a T-die method, the molten sheet extruded from the T-die may be stretched not only in the MD direction of the thermoplastic liquid crystal polymer film but also in both the TD direction and the MD direction simultaneously to form a film, or the molten sheet extruded from the T-die may be stretched in the MD direction once and then in the TD direction to form a film.
[0037] In addition, in extrusion molding by the inflation method, a cylindrical sheet melt-extruded from a ring die may be stretched at a predetermined draw ratio (corresponding to the stretch ratio in the MD direction) and blow ratio (corresponding to the stretch ratio in the TD direction) to form a film.
[0038] If necessary, a known or conventional heat treatment may be carried out to adjust the melting point and / or thermal expansion coefficient of the thermoplastic liquid crystal polymer film. The heat treatment conditions can be appropriately set depending on the purpose. For example, the melting point (Tm 0) with respect to (Tm 0 -10) ° C. or higher (for example, (Tm 0 -10) ° C ~ (Tm 0 +30)°C, preferably (Tm 0 ) ° C ~ (Tm 0 The melting point (Tm) of the thermoplastic liquid crystal polymer film may be increased by heating the film at a temperature of about +20°C for several hours. Depending on the composition of the thermoplastic liquid crystal polymer film, the melting point can be increased even with a shorter heating time, for example, one hour or less. 0 ) with respect to (Tm 0 -15)℃ or higher (Tm 0 The coefficient of thermal expansion may be increased by heating at a temperature of less than 10° C. for 5 to 60 seconds (eg, 10 to 30 seconds).
[0039] The melting point (Tm) of the thermoplastic liquid crystal polymer film may be, for example, 315°C or higher, preferably 315 to 380°C, more preferably 318 to 370°C, and even more preferably 320 to 360°C. The melting point (Tm) of the thermoplastic liquid crystal polymer film can be obtained by observing the thermal behavior of a thermoplastic liquid crystal polymer film sample using a differential scanning calorimeter. That is, a thermoplastic liquid crystal polymer film sample is heated from room temperature (e.g., 25°C) at a rate of 10°C / min until completely melted at 400°C, and then the melt is cooled to 50°C at a rate of 10°C / min, and the position of the endothermic peak that appears when the temperature is raised again at a rate of 10°C / min can be determined as the melting point (Tm) of the thermoplastic liquid crystal polymer film.
[0040] The thickness of the thermoplastic liquid crystal polymer film can be appropriately set depending on the application. For example, when considering use as a material for the insulating layer of a circuit board, it may be 10 to 500 μm, preferably 15 to 250 μm, more preferably 20 to 200 μm, and even more preferably 25 to 150 μm.
[0041] (Surface Roughness of Thermoplastic Liquid Crystal Polymer Film) In the present invention, the surface roughness of the thermoplastic liquid crystal polymer film is adjusted to improve the adhesion of conductive ink. Note that Sv, Sz, and Spk described below are all surface roughness parameters defined by ISO 25178 and can be measured by the method described in the Examples below. Maximum Valley Depth Sv: The thermoplastic liquid crystal polymer film of the present invention preferably has a surface roughness indicated by a maximum valley depth Sv of 0.15 μm or more and 2.0 μm or less on at least one surface. Here, the maximum valley depth Sv is the maximum depth from the reference plane (average height plane) of the surface irregularities to the valley bottom. If the maximum valley depth Sv is less than 0.15 μm, the effect of improving the adhesion of conductive ink cannot be obtained. If the maximum valley depth exceeds 2.0 μm, the adhesion and conductivity of the formed circuit will decrease. The Sv value is preferably 0.2 μm or more, more preferably greater than 0.4 μm, and even more preferably 0.5 μm or more. The Sv value is preferably 1.5 μm or less, and may be 1.0 μm or less. For example, Sv may be more than 0.4 μm and 2.0 μm or less.
[0042] In the thermoplastic liquid crystal polymer film, the maximum surface height Sz is preferably 2.5 μm or less, more preferably 2.0 μm or less. By suppressing Sz to a predetermined value or less, conductivity can be improved when a circuit is formed with conductive ink. The Sz value may be 1.5 μm or less or 0.5 μm or more.
[0043] In the thermoplastic liquid crystal polymer film, the ratio Sv / Sz of the maximum valley depth Sv to the maximum height Sz of the surface is preferably 0.6 or more and 1 or less, more preferably 0.7 or more and 1 or less.
[0044] Spk In the above-mentioned thermoplastic liquid crystal polymer film, the height Spk of the protruding peaks on the surface may be 0.03 μm or more and 0.40 μm or less. Having Spk within the above range can further reduce air entrapment when forming a circuit with conductive ink, further reduce the occurrence of voids after sintering and cracks when bending, and also provide better adhesion. The height Spk of the protruding peaks may be 0.10 μm or more, more preferably greater than 0.10 μm, for example, 0.11 μm or more. Spk may be 0.25 μm or less, or 0.2 μm or less. For example, Spk may be greater than 0.10 μm and 0.40 μm or less, or may be 0.11 μm or more and 0.25 μm or less.
[0045] (Method for preparing the surface roughness of a thermoplastic liquid crystal polymer film) The surface roughness of a thermoplastic liquid crystal polymer film can be formed, for example, by heat-treating a thermoplastic liquid crystal polymer film laminated on a support, then pressing the surface with the nip roll of a calendar roll to flatten the convex portions and make the valley shapes prominent.
[0046] A metal foil may be used as the support, and the laminate may be formed as a single-sided metal-clad laminate by a known method.
[0047] In the present invention, when a metal foil is used as a support for adjusting the surface roughness of the thermoplastic liquid crystal polymer film, a one-sided metal clad plate can be formed by a known method. The metal foil is not particularly limited, but aluminum or aluminum alloy foil, stainless steel foil, rolled copper foil, electrolytic copper foil, etc. can be used.
[0048] The thickness of the metal foil may be, for example, 1 to 100 μm, and the metal foil may be subjected to a surface roughening treatment. The thermoplastic liquid crystal polymer film and the metal foil can be thermocompression bonded using a pair of metal rolls, or a metal roll and a rubber roll, for example, by applying a pressure of about 1 to 15 kg / mm by a roll-to-roll method while heating at a heating temperature in the range of (Tm-80)°C to (Tm)°C relative to the melting point (Tm) of the thermoplastic liquid crystal polymer film.
[0049] During thermocompression bonding, the thermoplastic liquid crystal polymer film and metal foil may be stacked so that a protective material such as a polyimide film is in contact with the outside of the stacked film, and then introduced into a pair of pressure rolls to be thermocompressed, and then separated from the single-sided metal-clad laminate before the heat treatment process.
[0050] In the heat treatment step, the single-sided metal-clad laminate is heat-treated. The heat treatment step may be performed downstream of the thermocompression bonding step without winding, or may be performed after the thermocompression bonding step and then winding.
[0051] The heat treatment is preferably carried out by a non-contact heating means from the viewpoint of alleviating distortion of the thermoplastic liquid crystal polymer film. Examples of the heating means include known heating means such as atmospheric heating and radiation heating using electromagnetic waves such as infrared rays and microwaves, and examples of the heat source include a hot air oven, a steam oven, an electric heater, an infrared heater, a ceramic heater, and a microwave irradiator.
[0052] The heat treatment temperature is preferably a temperature equal to or higher than the melting point (Tm) of the thermoplastic liquid crystal polymer film. For example, the heat treatment may be performed at a temperature of Tm to Tm + 50°C, or in the range of Tm + 5°C to Tm + 30°C. The heat treatment time may be in the range of 10 to 180 seconds, preferably 15 to 120 seconds, and more preferably 20 to 90 seconds.
[0053] After the heat treatment, the film is passed through one or two pairs of metal rolls and nip pressure is applied at a predetermined temperature to flatten the peaks (protrusions) on the surface of the thermoplastic liquid crystal polymer film, adjusting the surface condition and controlling the values of Sv, Spk, Sz, etc. to the desired values. In this case, pressure may be applied with a protective film such as a polyimide film laminated on both sides of the single-sided metal-clad laminate. The heating temperature during pressure application is preferably a temperature below the melting point (Tm) of the thermoplastic liquid crystal polymer film, for example, Tm-130°C to Tm-5°C, preferably Tm-80°C to Tm-20°C, for example, about 200 to 270°C. The nip pressure may be, for example, 1.0 to 4.0 kg / mm in terms of linear pressure.
[0054] The laminate after the heat treatment is a one-sided metal-clad plate in which a metal foil is laminated on one side of the thermoplastic liquid crystal polymer film and the surface roughness of one side (film side) is adjusted. This laminate may be used as the laminate of the present invention described below, or the metal foil laminated as a support may be removed by etching and used as a thermoplastic liquid crystal polymer film.
[0055] (Laminate) The laminate of the present invention is a laminate including a thermoplastic liquid crystal polymer film having a maximum valley depth Sv of 1.5 μm or more and 2.0 μm or less on at least one surface, and a conductive layer laminated on at least one surface of the thermoplastic liquid crystal polymer film.
[0056] Here, one side of the thermoplastic liquid crystal polymer film is designated as the first side, and the opposite side is designated as the second side, with the first side being the side exhibiting the above-mentioned Sv value. The laminate may be a single-sided metal-clad plate with a metal foil laminated and pressure-bonded to the second side, or may have a conductive layer such as a circuit pattern formed on the first side using conductive ink. Alternatively, the first side may have a conductive layer formed on it using conductive ink, and the metal foil laminated as a support during surface roughness adjustment may be removed from the second side. Furthermore, a separate metal layer may be laminated on the second side from which the metal foil has been removed by means of sputtering or the like.
[0057] The pattern can be drawn using a conductive ink by, for example, drawing lines with a marker, drawing lines with an inkjet printer, or printing by screen printing, and is not particularly limited. Examples of conductive inks that can be used include water-based or oil-based inks containing metal particles such as Au, Pt, Ag, Cu, Ni, Cr, Rh, Pd, Zn, Co, Mo, Ru, W, Os, Ir, Fe, Mn, Ge, Sn, Ga, In, or alloys thereof. After drawing with the conductive ink, it is preferable to perform a heat treatment to sinter the metal particles. Sintering can be performed at a temperature of approximately 100 to 450°C, but the heat treatment temperature is preferably lower than the melting point of the thermoplastic liquid crystal polymer film used as the substrate.
[0058] In the present invention, the surface roughness of the first surface is adjusted in consideration of the adhesiveness of the conductive ink, but if necessary, a metal layer may be formed on the first surface by a method such as vapor deposition, sputtering, or electroless plating. In this case, a circuit may be formed on the metal layer by a known method.
[0059] The laminate of the present invention can be effectively used as a part used in the fields of electricity and electronics, office equipment and precision equipment, power semiconductors, etc., for example, as a circuit board material.
[0060] A circuit board using the laminate of the present invention is suitable for use as a high frequency circuit board, an in-vehicle sensor, a mobile circuit board, an antenna, and the like.
[0061] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the following examples and comparative examples, various physical properties were measured by the following methods.
[0062] [Melting Point] Using a differential scanning calorimeter (Shimadzu Corporation), a predetermined size sample was taken from the thermoplastic liquid crystal polymer film and placed in a sample container. The sample was heated from room temperature at a rate of 10°C / min until it was completely melted at 400°C. The melt was then cooled to 50°C at a rate of 10°C / min, and the temperature was raised again at a rate of 10°C / min. The position of the endothermic peak that appeared was determined as the melting point (Tm) of the thermoplastic liquid crystal polymer film.
[0063] [Sz, Sv, Spk] The surface roughness was measured in accordance with ISO 25178 using a white light confocal microscope (OPTELICS HYBRID (L)) manufactured by Lasertec Corporation, measuring the maximum height Sz, maximum valley depth Sv, and peak height Spk, and then the ratio of Sv / Sz was determined. A 50x objective lens was used in the laser microscope, with a resolution of 0.05 μm and a measurement range of an area of 74.24 μm × 74.24 μm (5512 μm 2) was measured at three locations, the center and both sides, of a 30 cm wide sample, and the arithmetic mean values of the Sz, Sv, and Spk values at these three locations were defined as the Sz, Sv, and Spk values. The obtained average values of Sz and Sv were used to calculate the ratio Sv / Sz of the maximum height Sz and the maximum valley depth Sv. In the white light confocal microscope measurement, if the measurement surface was not flat but curved, flatness correction was performed before calculating the above surface properties. The measurement environment using the white light confocal microscope was a temperature of 23±2°C and a humidity of 50%±5%.
[0064] [Conductivity Evaluation] Three linear patterns, 1 mm wide and 100 mm long, were created on a thermoplastic liquid crystal polymer film by screen printing using silver paste (NPS manufactured by Harima Chemical Group Co., Ltd.), and then baked at 120°C for 1 hour to create a circuit pattern. The resistance of the created circuit pattern was measured using a digital multimeter RD700 manufactured by Sanwa Corporation to confirm the presence or absence of conductivity. The conductivity was evaluated as follows: ○ if all three lines were conductive, △ if two or fewer lines were conductive, and × if all three lines were conductive.
[0065] [MIT Test (Bending Test)] A wiring pattern with L (line) / S (space) = 1 / 1 mm was printed on the surface of the liquid crystal polymer, and the number of bending times was measured using an MIT folding endurance tester (MID-D, manufactured by Toyo Seiki Seisaku-sho, Ltd.) in accordance with JIS P 8115 at a rotation speed of 175 cpm, a measuring load of 500 g, a bending angle of 135°, and a bending curvature R of 0.38 mm, to perform bending evaluation.
[0066] Reference Example 1 [Preparation of single-sided copper-clad laminate] A copolymer of p-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid (molar ratio: 80 / 20) was heated and kneaded in an extruder, and then heated and kneaded at 280 to 340 ° C using an extruder. The mixture was then extruded through an inflation die with a diameter of 40 mm and a slit spacing of 0.6 mm to obtain a thermoplastic liquid crystal polymer film with a thickness of 50 μm. The melting point Tm of this thermoplastic liquid crystal polymer film was 320 ° C.
[0067] The obtained thermoplastic liquid crystal polymer film and copper foil (JX Nippon Mining Corporation: JXEFL-BHM foil, thickness 12 μm) were laminated by a roll-to-roll method. During lamination, a heated metal roll and a heat-resistant rubber roll were used, and the surface temperature of the heated metal roll was set to 280°C. In addition, the pressure applied to the thermoplastic liquid crystal polymer film and copper foil between the heat-resistant rubber roll and the heated metal roll was 40 kg / cm in terms of surface pressure. 2 Under these conditions, the thermoplastic liquid crystal polymer film was first moved along a heat-resistant rubber roll, and then the copper foil was temporarily bonded to the thermoplastic liquid crystal polymer film. The prepared laminate was passed through an IR heat treatment device (manufactured by Noritake Co., Ltd., product name: roll-to-roll far-infrared heating furnace) and subjected to heat treatment to prepare a single-sided copper-clad laminate of Reference Example 1.
[0068] Example 1 Polyimide films (Kaneka Corporation, "Apical" 50 μm) were placed on the top and bottom of the single-sided copper-clad plate material of Reference Example 1 as protective materials, and the plate was moved between two pairs of heated metal rolls to adjust the surface roughness of the thermoplastic liquid crystal polymer film surface. At this time, the heating temperature of the heated roll was 200 ° C, and the nip pressure was 3.7 kg / mm. The copper foil of this single-sided copper-clad laminate was removed by etching to obtain a thermoplastic liquid crystal polymer film alone. The surface roughness of the surface with the adjusted surface roughness is shown in Table 7.
[0069] Example 2 A thermoplastic liquid crystal polymer film with an adjusted surface roughness was produced in the same manner as in Example 1, except that the heating temperature of the heating roll was set to 220°C.
[0070] Example 3 A thermoplastic liquid crystal polymer film with an adjusted surface roughness was produced in the same manner as in Example 1, except that the heating temperature of the heating roll was set to 240°C.
[0071] Example 4 A thermoplastic liquid crystal polymer film with an adjusted surface roughness was produced in the same manner as in Example 1, except that the heating temperature of the heating roll was set to 260°C.
[0072] Example 5 A thermoplastic liquid crystal polymer film with an adjusted surface roughness was produced in the same manner as in Example 1, except that the heating temperature of the heating roll was set to 270°C.
[0073] Example 6 A thermoplastic liquid crystal polymer film with an adjusted surface roughness was produced in the same manner as in Example 1, except that the heating temperature of the heating roll was set to 250°C.
[0074] Comparative Example 1 Using the single-sided copper-clad laminate prepared in Reference Example 1 as a substrate, a thermoplastic liquid crystal polymer film having a solvent-cast surface was prepared. A 0.2 wt% copolymer of p-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid (molar ratio: 80 / 20) was added to a PFP (pentafluorophenol) solution and dissolved with stirring at 90°C to obtain a cloudy white solution. The solution was then degassed and cast onto the thermoplastic liquid crystal polymer film surface of the single-sided copper-clad laminate using a film applicator. The solution was then dried at 100°C for 24 hours and then at 200°C for 1 hour to produce a single-sided copper-clad laminate with a solvent-cast surface. The copper foil was then removed by chemical etching to obtain a film alone. The surface roughness of the solvent-cast surface is shown in Table 7.
[0075] Comparative Example 2 A thermoplastic liquid crystal polymer film with an adjusted surface roughness was produced in the same manner as in Example 1, except that the heating temperature of the heating roll was 280° C. and the nip pressure was 2.8 kg / mm.
[0076] Comparative Example 3 A thermoplastic liquid crystal polymer film with an adjusted surface roughness was produced in the same manner as in Example 1, except that the heating temperature of the heating roll was set to 280°C.
[0077] Comparative Example 4 The metal foil of the single-sided copper-clad laminate of Reference Example 1 was removed by etching to obtain a thermoplastic liquid crystal polymer film of Comparative Example 4. The surface roughness of the thermoplastic liquid crystal polymer film on the side opposite to the side from which the metal foil was removed by etching is shown in Table 7.
[0078] Comparative Example 5 Using a 1000 mesh buff roll with silicon carbide abrasive attached to nylon fibers, the thermoplastic liquid crystal polymer film surface of the single-sided copper-clad laminate of Reference Example 1 was buffed at a rotation speed of 2000 rpm and a conveying speed of 1 m / min. The copper foil was then removed by etching to obtain the thermoplastic liquid crystal polymer film of Comparative Example 5. The surface roughness of the buffed surface of the thermoplastic liquid crystal polymer film is shown in Table 7.
[0079] The thermoplastic liquid crystal polymer films of Examples 1 to 6 and Comparative Examples 1 to 5 were subjected to the above-described methods for measuring the surface roughness and for evaluating the conductive marker (evaluation of conductivity and number of bending times). The results are shown in Table 7.
[0080]
[0081] As shown in Table 7, Examples 1 to 6, in which the maximum valley depth Sv is within the range of the present invention, show good results in both conductivity and flex resistance (number of flexes), whereas Comparative Examples 1 to 5, in which the Sv value is outside the range of the present invention, show reduced flex resistance of the formed circuit.
[0082] The liquid crystal polymer film of the present invention and a liquid crystal polymer molded article containing the same can be easily processed into circuits using conductive ink and can be effectively used as a circuit board material with excellent high-frequency characteristics, and therefore are highly applicable in industrial fields such as printed electronics.
[0083] While the preferred embodiments of the present invention have been described above, those skilled in the art will readily recognize various changes and modifications within the scope of the present invention, which are obvious from the description of the present invention. Therefore, such changes and modifications are to be interpreted as falling within the scope of the invention as defined by the claims.
Claims
1. A thermoplastic liquid crystal polymer film comprising a polymer capable of forming an optically anisotropic molten phase (hereinafter referred to as a thermoplastic liquid crystal polymer), wherein the maximum valley depth Sv on at least one surface is 0.15 μm or more and 2.0 μm or less.
2. A thermoplastic liquid crystal polymer film according to claim 1, wherein the maximum height Sz of the surface is 2.5 μm or less.
3. A thermoplastic liquid crystal polymer film according to claim 1 or 2, in which the ratio Sv / Sz of the maximum valley depth Sv to the maximum height Sz of the surface is 0.6 or more and 1 or less.
4. A thermoplastic liquid crystal polymer film according to claim 1 or 2, wherein the height Spk of the protruding peaks on the surface is 0.03 μm or more and 0.40 μm or less.
5. A thermoplastic liquid crystal polymer film according to claim 1 or 2, having a melting point of 315°C or higher.
6. A laminate comprising the thermoplastic liquid crystal polymer film according to claim 1 or 2 and a conductive layer laminated on at least one surface of the film.
7. A laminate according to claim 6, in which a layer composed of at least one material selected from the group consisting of conductive ink, metal film, and circuits formed therefrom is formed on the surface of the thermoplastic liquid crystal polymer film as a conductive layer.
8. A laminate according to claim 7, wherein a metal foil layer is formed as a conductive layer on the surface opposite to the surface of the thermoplastic liquid crystal polymer film.
9. The laminate according to claim 6, which is a circuit board.
Citation Information
Patent Citations
Resin sheet and resin laminate substrate
JP2019104157A
Substrate for printed wiring board and method for manufacturing same, printed wiring board and method for manufacturing same, and resin base material
WO2016104420A1
Thermoplastic liquid crystal polymer molded article
WO2021251261A1