Thermoplastic liquid crystal polymer film, laminate, and methods for producing same

The thermoplastic liquid crystal polymer film with controlled surface roughness addresses adhesion and frequency challenges by optimizing surface treatment, resulting in improved adhesion and low transmission loss for flexible circuit boards.

WO2024204238A1PCT designated stage expired Publication Date: 2024-10-03KURARAY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012021
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-26
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing thermoplastic liquid crystal polymer films face challenges in achieving good adhesion with metal layers and maintaining high frequency characteristics, particularly in flexible circuit boards, due to surface roughness issues and residual copper particles that act as nuclei for crystal growth, leading to non-uniform metal layers and increased transmission loss.

Method used

A thermoplastic liquid crystal polymer film with controlled surface roughness, characterized by a skewness of -5 to 0 and an arithmetic mean roughness of 0.15 μm or more, is developed by adjusting the surface treatment conditions using a roll, ensuring excellent adhesion and low transmission loss when laminated with a conductor layer.

Benefits of technology

The film achieves both good adhesion to the conductor layer and low transmission loss, enabling effective circuit processability and high-frequency performance in flexible circuit boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure WO-DOC-TABLE-4
    Figure WO-DOC-TABLE-4
  • Figure WO-DOC-TABLE-5
    Figure WO-DOC-TABLE-5
  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

The thermoplastic liquid crystal polymer film contains a polymer capable of forming an optically anisotropic molten phase, wherein, on at least one surface, the skewness (bias) Ssk is -5 to 0 inclusive, and the arithmetic mean roughness Sa of the surface is 0.15 μm or more.
Need to check novelty before this filing date? Find Prior Art

Description

Thermoplastic liquid crystal polymer film, laminate, and method for producing same Related Applications

[0001] This application claims priority from Japanese Patent Application No. 2023-053939, filed March 29, 2023, the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to a thermoplastic liquid crystal polymer film containing a polymer capable of forming an optically anisotropic melt phase (hereinafter referred to as a thermoplastic liquid crystal polymer), a laminate containing the thermoplastic liquid crystal polymer film, and a method for producing the thermoplastic liquid crystal polymer film and the laminate.

[0003] In recent years, the use of flexible circuit boards consisting of laminates of resin and metal layers has been increasing in the field of electronic materials. Thermoplastic liquid crystal polymer films are known as materials with excellent heat resistance, low moisture absorption, and high-frequency characteristics, and have recently attracted attention as flexible circuit board materials for high-speed transmission.

[0004] In response to demands for smaller, higher-density circuits in flexible circuit boards, finer circuit patterns are being developed, and the semi-additive process (SAP process) is being considered as a technology that enables fine circuit processing. For example, Patent Document 1 (WO 2020 / 105289) describes a technology for suppressing the occurrence of intercalation in the plating layer during the process of etching an electroless copper plating layer formed on the surface of a base resin film by thermocompression bonding a surface-treated copper foil and a resin film to transfer the surface shape of the surface-treated copper foil to the surface of the resin film, and then removing the surface-treated copper foil by etching, thereby reducing the skewness Ssk, measured in accordance with ISO 25178, on the surface of the remaining resin film to −0.6 or less.

[0005] International Publication No. 2020 / 105289

[0006] In flexible circuit boards, good adhesion is required between the resin layer and the metal layer (conductor layer), and in order to exhibit the high-frequency characteristics of the thermoplastic liquid crystal polymer film, it is preferable that a smooth interface exists between the resin layer and the metal layer.

[0007] The technology of Patent Document 1 involves thermocompression bonding a resin film to the treated surface of a surface-treated copper foil to transfer the surface shape of the treated surface to the surface of the resin film, and then removing the surface-treated copper foil by etching, thereby achieving a skewness Ssk of -0.6 or less on the surface of the resin film. However, this method makes it difficult to create a flat surface on the surface of the resin film. Patent Document 1 also uses a film made of a thermosetting resin, but with a thermoplastic liquid crystal polymer film that has low moisture absorption, it is difficult to completely etch out the copper embedded in the valleys of the film surface. Furthermore, if copper remains partially on the surface of the thermoplastic liquid crystal polymer film, it becomes a nucleus for crystal growth, making it difficult to form a uniform metal layer in a subsequent plating process.

[0008] The present invention aims to provide a thermoplastic liquid crystal polymer film that can reduce transmission loss when laminated with a metal layer and has good adhesion to the metal layer, a laminate containing such a thermoplastic liquid crystal polymer film, and methods for manufacturing these.

[0009] As a result of intensive research to achieve the above-mentioned objective, the inventors of the present invention discovered that by adjusting the conditions when treating the surface of a thermoplastic liquid crystal polymer film with a roll, the film can be given a surface roughness that results in a skewness within a predetermined range, thereby achieving both adhesion to a conductor layer and maintaining high-frequency characteristics, and thus completed the present invention.

[0010] That is, the present invention can be configured in the following aspects. [Aspect 1] A thermoplastic liquid crystal polymer film containing a polymer capable of forming an optically anisotropic melt phase (hereinafter referred to as a thermoplastic liquid crystal polymer), wherein at least one surface of the thermoplastic liquid crystal polymer film has a skewness (degree of bias) Ssk of -5 or more and 0 or less (preferably less than 0, more preferably -0.2 or less), and the arithmetic mean roughness Sa of the surface is 0.15 μm or more. [Aspect 2] The thermoplastic liquid crystal polymer film according to Aspect 1, wherein the surface is metal-free.

[0011] [Aspect 3] The thermoplastic liquid crystal polymer film according to aspect 1 or 2, wherein the arithmetic mean roughness Sa of the surface is 0.50 μm or less (preferably 0.15 μm or more and 0.50 μm or less, for example 0.15 μm or more and 0.30 μm or less, or 0.20 μm or more and 0.50 μm or less). [Aspect 4] The thermoplastic liquid crystal polymer film according to any one of aspects 1 to 3, wherein the maximum peak height Sp of the surface is 0.15 μm or more (preferably 0.5 μm or more) and 3.00 μm or less.

[0012] [Aspect 5] The thermoplastic liquid crystal polymer film according to any one of Aspects 1 to 4, wherein the maximum valley depth Sv of the surface is 0.2 μm or more and 3.5 μm or less (preferably 1.0 μm or more and 3.0 μm or less). [Aspect 6] The thermoplastic liquid crystal polymer film according to any one of Aspects 1 to 5, wherein the maximum height Sz of the surface is 1.5 μm or more and 5.0 μm or less. [Aspect 7] The thermoplastic liquid crystal polymer film according to any one of Aspects 1 to 6, wherein the melting point is 315° C. or more.

[0013] [Aspect 8] A laminate comprising the thermoplastic liquid crystal polymer film according to any one of Aspects 1 to 7 and a conductive layer laminated on the thermoplastic liquid crystal polymer film. [Aspect 9] The laminate according to Aspect 8, wherein a layer composed of at least one selected from the group consisting of conductive ink, metal film, and circuits formed therefrom is formed on the surface of the thermoplastic liquid crystal polymer film as a conductive layer. [Aspect 10] The laminate according to Aspect 8 or 9, wherein a metal foil layer is formed as a conductive layer on the surface opposite to the surface of the thermoplastic liquid crystal polymer film.

[0014] [Aspect 11] The laminate according to any one of Aspects 8 to 10, wherein the laminate is a circuit board. [Aspect 12] A method for producing the thermoplastic liquid crystal polymer film according to any one of Aspects 1 to 7, comprising at least a step of contacting at least one surface of the thermoplastic liquid crystal polymer film with a roughened surface roll.

[0015] [Aspect 13] The method for producing a laminate according to any one of Aspects 8 to 11, comprising at least a step of contacting a surface of the thermoplastic liquid crystal polymer film of a laminate of the thermoplastic liquid crystal polymer film and a support with a roll having a roughened surface. [Aspect 14] The method for producing a laminate according to Aspect 13, wherein the support is a metal foil.

[0016] It should be noted that any combination of at least two elements disclosed in the claims and / or the specification is included in the present invention, and in particular any combination of two or more of the claims described in the claims is included in the present invention.

[0017] According to the thermoplastic liquid crystal polymer film of the present invention, when laminated with a conductor layer, it is possible to obtain a thermoplastic liquid crystal polymer film that can keep transmission loss low and has good adhesion to the conductor layer, and a laminate containing such a thermoplastic liquid crystal polymer film has excellent circuit processability.

[0018] (Thermoplastic liquid crystal polymer film) The thermoplastic liquid crystal polymer film includes a thermoplastic liquid crystal polymer. The thermoplastic liquid crystal polymer is composed of a melt-moldable liquid crystal polymer (or a polymer capable of forming an optically anisotropic molten phase), and its chemical structure is not particularly limited as long as it is a melt-moldable liquid crystal polymer. For example, a thermoplastic liquid crystal polyester or a thermoplastic liquid crystal polyester amide in which an amide bond is introduced therein can be mentioned.

[0019] The thermoplastic liquid crystal polymer may also be a polymer in which an isocyanate-derived bond such as an imide bond, a carbonate bond, a carbodiimide bond or an isocyanurate bond is further introduced into an aromatic polyester or an aromatic polyester amide.

[0020] Specific examples of the thermoplastic liquid crystal polymer used in the present invention include known thermoplastic liquid crystal polyesters and thermoplastic liquid crystal polyester amides derived from the compounds classified as (1) to (4) shown below and their derivatives. However, it goes without saying that there is an appropriate range for the combination of various raw material compounds in order to form a polymer that can form an optically anisotropic molten phase.

[0021] (1) Aromatic or aliphatic diol (see Table 1 for representative examples)

[0022] (2) Aromatic or aliphatic dicarboxylic acids (see Table 2 for representative examples)

[0023] (3) Aromatic hydroxycarboxylic acids (see Table 3 for representative examples)

[0024] [Amendment under Rule 91 17.07.2024] (4) Aromatic diamines, aromatic hydroxyamines or aromatic aminocarboxylic acids (see Table 4 for representative examples)

[0025] Representative examples of thermoplastic liquid crystal polymers obtained from these raw material compounds include copolymers having the repeating units shown in Tables 5 and 6.

[0026] [Amendment under Rule 91 17.07.2024] [Table 6]

[0027] Among these copolymers, copolymers containing at least p-hydroxybenzoic acid and / or 6-hydroxy-2-naphthoic acid as repeating units are preferred, and particularly preferred are (i) copolymers containing repeating units of p-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid, or (ii) copolymers containing repeating units of at least one aromatic hydroxycarboxylic acid selected from the group consisting of p-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid, at least one aromatic diol and / or aromatic hydroxyamine, and at least one aromatic dicarboxylic acid.

[0028] For example, in the copolymer (i), when the thermoplastic liquid crystal polymer contains at least repeating units of p-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid, the molar ratio (A) / (B) of the p-hydroxybenzoic acid in the repeating unit (A) to the 6-hydroxy-2-naphthoic acid in the repeating unit (B) in the thermoplastic liquid crystal polymer is preferably about (A) / (B) = 10 / 90 to 90 / 10, more preferably about (A) / (B) = 15 / 85 to 85 / 15, and even more preferably about (A) / (B) = 20 / 80 to 80 / 20.

[0029] In the case of the copolymer (i), in addition to the repeating units of p-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid, from the viewpoint of adjusting the molecular weight, etc., it may contain repeating units composed of an aromatic diol or an aromatic dicarboxylic acid (for example, terephthalic acid).

[0030] In the case of the copolymer (ii), at least one aromatic hydroxycarboxylic acid (C) selected from the group consisting of p-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid, at least one aromatic diol (D) selected from the group consisting of 4,4'-dihydroxybiphenyl, hydroquinone, phenylhydroquinone, and 4,4'-dihydroxydiphenyl ether, and at least one aromatic dicarboxylic acid (E) selected from the group consisting of terephthalic acid, isophthalic acid, and 2,6-naphthalenedicarboxylic acid. The molar ratio of each repeating unit of the aromatic hydroxycarboxylic acid (C): the aromatic diol (D): the aromatic dicarboxylic acid (E) in the thermoplastic liquid crystal polymer may be about (30 to 80): (35 to 10): (35 to 10), more preferably about (C): (D): (E) = (35 to 75): (32.5 to 12.5): (32.5 to 12.5), and even more preferably about (C): (D): (E) = (40 to 70): (30 to 15): (30 to 15).

[0031] The molar ratio of repeating units derived from 6-hydroxy-2-naphthoic acid in the aromatic hydroxycarboxylic acid (C) may be, for example, 85 mol % or more, preferably 90 mol % or more, and more preferably 95 mol % or more. The molar ratio of repeating units derived from 2,6-naphthalenedicarboxylic acid in the aromatic dicarboxylic acid (E) may be, for example, 85 mol % or more, preferably 90 mol % or more, and more preferably 95 mol % or more.

[0032] Alternatively, the aromatic diol (D) may be repeating units (D1) and (D2) derived from two different aromatic diols selected from the group consisting of hydroquinone, 4,4'-dihydroxybiphenyl, phenylhydroquinone, and 4,4'-dihydroxydiphenyl ether. In this case, the molar ratio of the two aromatic diols (D1) / (D2) may be 23 / 77 to 77 / 23, more preferably 25 / 75 to 75 / 25, and even more preferably 30 / 70 to 70 / 30.

[0033] Furthermore, the molar ratio of the repeating structural units derived from the aromatic diol to the repeating structural units derived from the aromatic dicarboxylic acid, (D) / (E), is preferably 95 / 100 to 100 / 95. If the ratio is outside this range, the degree of polymerization does not increase and the mechanical strength tends to decrease.

[0034] The ability to form an optically anisotropic molten phase in the present invention can be confirmed, for example, by placing a sample on a hot stage, heating it in a nitrogen atmosphere, and observing the light transmitted through the sample.

[0035] Melting point of thermoplastic liquid crystal polymer (Tm 0) is preferably in the range of 300 to 380 ° C, more preferably in the range of 305 to 360 ° C, and even more preferably in the range of 310 to 350 ° C. The melting point of the thermoplastic liquid crystal polymer can be obtained by observing the thermal behavior of the thermoplastic liquid crystal polymer sample using a differential scanning calorimeter. That is, the thermoplastic liquid crystal polymer sample is heated at a rate of 10 ° C / min until it is completely melted, and then the melt is cooled to 50 ° C at a rate of 10 ° C / min, and the position of the endothermic peak that appears after heating again at a rate of 10 ° C / min is recorded as the melting point of the thermoplastic liquid crystal polymer sample.

[0036] Furthermore, from the viewpoint of melt moldability, the thermoplastic liquid crystal polymer is, for example, 0 The melt viscosity at a shear rate of 1000 / s at +20°C may be 30 to 120 Pa·s, and preferably 50 to 100 Pa·s.

[0037] The thermoplastic liquid crystal polymer film may contain a thermoplastic polymer such as polyethylene terephthalate, modified polyethylene terephthalate, polyolefin, polycarbonate, polyarylate, polyamide, polyphenylene sulfide, polyether ether ketone, or fluororesin, as well as various additives, within the scope of the present invention. Furthermore, it may contain a filler such as an organic filler or an inorganic filler, as necessary. Therefore, the thermoplastic liquid crystal polymer film of the present invention also includes a film made of a thermoplastic liquid crystal polymer composition containing a thermoplastic liquid crystal polymer as a main component and one or more of these heterogeneous polymers, additives, fillers, etc.

[0038] The thermoplastic liquid crystal polymer film may contain 50% by weight or more of thermoplastic liquid crystal polymer, preferably 80% by weight or more, more preferably 90% by weight or more, even more preferably 95% by weight or more, and even more preferably 98% by weight or more.

[0039] The thermoplastic liquid crystal polymer film may be an extrusion film obtained by extruding the above-mentioned thermoplastic liquid crystal polymer or thermoplastic liquid crystal polymer film composition.At this time, any extrusion molding method can be used, but the well-known T-die film stretching method, laminate stretching method, inflation method, etc. are industrially advantageous.In particular, in the inflation method, stress is applied not only in the mechanical axis direction (hereinafter referred to as MD direction) of the thermoplastic liquid crystal polymer film, but also in the direction perpendicular thereto (hereinafter referred to as TD direction), and it can be uniformly stretched in the MD direction and the TD direction, so that a thermoplastic liquid crystal polymer film with controlled molecular orientation, dielectric properties, etc. can be obtained.

[0040] In addition, the thermoplastic liquid crystal polymer film may be stretched as needed after extrusion molding.The stretching method itself is known, and either biaxial stretching or uniaxial stretching may be adopted, but biaxial stretching is preferred because it is easier to control the molecular orientation degree.In addition, for stretching, known uniaxial stretching machines, simultaneous biaxial stretching machines, sequential biaxial stretching machines, etc. can be used.

[0041] In extrusion molding, a stretching process may be performed to control the orientation. For example, in extrusion molding using a T-die method, the molten sheet extruded from the T-die may be stretched not only in the MD direction of the thermoplastic liquid crystal polymer film but also in both the TD direction and the MD direction simultaneously to form a film, or the molten sheet extruded from the T-die may be stretched in the MD direction once and then in the TD direction to form a film.

[0042] In addition, in extrusion molding by the inflation method, a cylindrical sheet melt-extruded from a ring die may be stretched at a predetermined draw ratio (corresponding to the stretch ratio in the MD direction) and blow ratio (corresponding to the stretch ratio in the TD direction) to form a film.

[0043] If necessary, a known or conventional heat treatment may be carried out to adjust the melting point and / or thermal expansion coefficient of the thermoplastic liquid crystal polymer film. The heat treatment conditions can be appropriately set depending on the purpose. For example, the melting point (Tm 0 ) with respect to (Tm 0 -10) ° C. or higher (for example, (Tm 0-10) ° C ~ (Tm 0 +30)°C, preferably (Tm 0 ) ° C ~ (Tm 0 The melting point (Tm) of the thermoplastic liquid crystal polymer film may be increased by heating the film at a temperature of about +20°C for several hours. Depending on the composition of the thermoplastic liquid crystal polymer film, the melting point can be increased even with a shorter heating time, for example, one hour or less. 0 ) with respect to (Tm 0 -15)℃ or higher (Tm 0 The coefficient of thermal expansion may be increased by heating at a temperature of less than 10° C. for 5 to 60 seconds (eg, 10 to 30 seconds).

[0044] The melting point (Tm) of the thermoplastic liquid crystal polymer film may be, for example, 315°C or higher, preferably 315 to 380°C, more preferably 318 to 370°C, and even more preferably 320 to 360°C. The melting point (Tm) of the thermoplastic liquid crystal polymer film can be obtained by observing the thermal behavior of a thermoplastic liquid crystal polymer film sample using a differential scanning calorimeter. That is, a thermoplastic liquid crystal polymer film sample is heated from room temperature (e.g., 25°C) at a rate of 10°C / min until completely melted at 400°C, and then the melt is cooled to 50°C at a rate of 10°C / min, and the position of the endothermic peak that appears when the temperature is raised again at a rate of 10°C / min can be determined as the melting point (Tm) of the thermoplastic liquid crystal polymer film.

[0045] The thickness of the thermoplastic liquid crystal polymer film can be appropriately set depending on the application. For example, when considering use as a material for the insulating layer of a circuit board, it may be 10 to 500 μm, preferably 15 to 250 μm, more preferably 20 to 200 μm, and even more preferably 25 to 150 μm.

[0046] (Surface Roughness of Thermoplastic Liquid Crystal Polymer Film) In the present invention, in order to improve adhesion with the metal layer, the surface roughness of the thermoplastic liquid crystal polymer film is adjusted by the following parameters. These are all parameters specified in ISO 25178 and are measured by the method described in the examples below.

[0047] Skewness (degree of bias) Ssk At least one surface of the thermoplastic liquid crystal polymer film of the present invention has a skewness Ssk of -5 or more and 0 or less. Skewness is a parameter that indicates the symmetry of the height distribution with respect to a reference plane, and when Ssk is less than 0, there are many valleys. Skewness Ssk is preferably less than 0, and more preferably -0.2 or less. Skewness Ssk may be -0.5 or more and 0 or less, or -5 or more and -2 or less.

[0048] Arithmetic mean roughness Sa Furthermore, the thermoplastic liquid crystal polymer film of the present invention has an arithmetic mean roughness Sa of 0.15 μm or more on the surface where the Ssk is -5 or more and 0 or less. If Sa is less than 0.15 μm, good peel strength may not be achieved by plating or vapor deposition. Furthermore, the arithmetic mean roughness Sa is preferably 0.50 μm or less. The arithmetic mean roughness Sa may be 0.15 μm or more and 0.30 μm or less, or may be 0.20 μm or more and 0.50 μm or less. When the Ssk of at least one surface of the thermoplastic liquid crystal polymer film is -5 or more and 0 or less, and Sa is 0.15 μm or more, both peel strength and transmission characteristics can be achieved.

[0049] In addition to the skewness and arithmetic mean roughness, it is preferable to adjust the following surface roughness parameters: Maximum peak height Sp The maximum peak height Sp of the surface is preferably 0.15 μm or more and 3.0 μm or less. The maximum peak height Sp is more preferably 0.5 μm or more. The maximum peak height Sp may be 0.5 μm or more and 1.0 μm or less, or may be 2.0 μm or more and 3.0 μm or less.

[0050] The maximum valley depth Sv of the surface is preferably 0.2 μm or more and 3.5 μm or less, more preferably 1.0 μm or more and 3.0 μm or less, and even more preferably 1.5 μm or more and 2.0 μm or less.

[0051] Maximum height Sz The maximum height Sz of the surface is preferably 1.5 μm or more and 5.0 μm or less. The maximum valley depth Sz is more preferably 2.0 μm or more. The maximum valley depth Sz may be 2.0 μm or more and 3.0 μm or less, or may be 3.5 μm or more and 5.0 μm or less.

[0052] Kurtosis Sku The kurtosis Sku may be 1.0 or more and 40.0 or less, preferably 1.5 or more and 30.0 or less, and more preferably 2.5 or more and 20.0 or less.

[0053] (Method for Adjusting the Surface Roughness of a Thermoplastic Liquid Crystal Polymer Film) The surface roughness of a thermoplastic liquid crystal polymer film can be adjusted by any of the following methods, or a combination of them. (1) Adjusting the Peripheral Speed ​​of the Heating Roll with Respect to the Film Conveying Speed ​​When a film is conveyed along a heating roll (e.g., a metal roll), changing the peripheral speed of the heating roll with respect to the film conveying speed can generate distortion on the film surface and adjust the surface roughness. The ratio of the peripheral speed of the heating roll with respect to the film conveying speed (film conveying speed / heating roll peripheral speed) is preferably 0.95 or more and 0.99 or less. (2) Film Shrinkage on the Heating Roll When a film is conveyed along a crown heating roll, tension is generated in the film from both ends toward the center, which can cause wrinkles to form in the film. In this case, the peaks on the film surface are pressed and crushed by the roll, forming a surface with predominant valleys. Note that wrinkles can be efficiently generated by using a thermoplastic liquid crystal polymer film with a negative thermal expansion coefficient in the TD direction. This process may be carried out while heating the film at a temperature of about Tm-110° C. to Tm-5° C., where Tm is the melting point of the thermoplastic liquid crystal polymer film.

[0054] (3) Transfer of the Roughened Surface of a Surface-Roughened Roll When a film is conveyed along a surface-roughened heated roll, the roughened surface of the heated roll is transferred to the surface of the thermoplastic liquid crystal polymer film. In this case, for example, by using a metal roll embossed with a linear pattern as the heated roll, a surface consisting of flat surfaces and valleys can be imparted to the thermoplastic liquid crystal polymer film. In this case, the preferred ranges of the surface roughness of the metal roll, measured in accordance with JIS B 0601:2001, are an arithmetic mean roughness Ra of 0.2 to 3.0 μm, a maximum height roughness Rz of 0.4 to 20.0 μm, and a ten-point mean roughness Rzjis of 0.3 to 20.0 μm. The temperature of the heated roll may be approximately Tm-110°C to Tm-5°C, where Tm is the melting point of the thermoplastic liquid crystal polymer film.

[0055] (4) Pressing with a Surface-Roughened Roll When a film is sandwiched between two rolls and conveyed while being pressed, at least one of the rolls can be roughened to transfer the roughened surface of the roll to the film surface, resulting in the desired roughened surface. In this method, for example, a rubber roll that has been surface-treated by embossing or the like, or a metal roll that has been surface-roughened by sandblasting or the like, can be used. This process may be carried out while heating the film at a temperature of about Tm-80°C to Tm-5°C relative to the melting point Tm of the thermoplastic liquid crystal polymer film. For example, the film may be heated with a metal heating roll while being pressed with a surface-roughened rubber roll.

[0056] As a method for adjusting the surface roughness of the thermoplastic liquid crystal polymer film, a method is known in which a metal foil having a predetermined surface roughness is laminated and pressed onto the thermoplastic liquid crystal polymer film, and then the metal foil is removed by etching.However, in this case, metal residue may remain on the surface of the thermoplastic liquid crystal polymer film.In contrast, the above-mentioned method can make the surface of the thermoplastic liquid crystal polymer film metal-free without leaving any metal residue on the surface of the thermoplastic liquid crystal polymer film.

[0057] The surface roughness of the thermoplastic liquid crystal polymer film may be adjusted when the thermoplastic liquid crystal polymer film is used alone, or when a support is laminated on one side of the thermoplastic liquid crystal polymer film and the surface roughness of the other side is adjusted. For example, a single-sided metal-clad laminate may be prepared by laminating a metal foil on one side of the thermoplastic liquid crystal polymer film, and then the surface of the thermoplastic liquid crystal polymer film may be roughened. Alternatively, in the thermocompression bonding process between the metal foil and the thermoplastic liquid crystal polymer film, a surface-roughened roll may be used as the roll on the thermoplastic liquid crystal polymer film side, and the preparation of the single-sided metal-clad laminate and the surface roughening of the thermoplastic liquid crystal polymer film side may be performed simultaneously.

[0058] In the present invention, when a metal foil is used as a support for adjusting the surface roughness of the thermoplastic liquid crystal polymer film, a single-sided metal-clad laminate can be formed by a known method. The metal foil is not particularly limited, but aluminum or aluminum alloy foil, stainless steel foil, rolled copper foil, electrolytic copper foil, etc. can be used.

[0059] The thickness of the metal foil may be, for example, 1 to 100 μm, and the metal foil may be subjected to a surface roughening treatment. The thermoplastic liquid crystal polymer film and the metal foil can be thermocompression bonded using a pair of metal rolls, or a metal roll and a rubber roll, for example, by applying a pressure of about 1 to 15 kg / mm ​​by a roll-to-roll method while heating at a heating temperature in the range of (Tm-80)°C to (Tm)°C relative to the melting point (Tm) of the thermoplastic liquid crystal polymer film.

[0060] During thermocompression bonding, the thermoplastic liquid crystal polymer film and the metal foil may be superposed so that a protective material such as a polyimide film is in contact with the outside of the superposed thermoplastic liquid crystal polymer film and the metal foil, and then introduced into a pair of pressure rolls for thermocompression bonding, and then separated from the single-sided metal-clad laminate before the heat treatment step. However, when adjusting the surface roughness of the thermoplastic liquid crystal polymer film and thermocompression bonding are performed simultaneously, no protective material is provided on the thermoplastic liquid crystal polymer film side.

[0061] (Laminate) The laminate of the present invention (hereinafter sometimes referred to as laminate) is a laminate including a thermoplastic liquid crystal polymer film having, on at least one surface, a skewness Ssk of -5 or more and an arithmetic mean roughness Sa of 0.15 μm or more.

[0062] Here, one side of the thermoplastic liquid crystal polymer film is the first side, and the other side is the second side, and if the first side is the side that exhibits the above Ssk value and Sa value, the laminate may be one in which a metal layer (metal coating) is formed on the first side by a method such as vapor deposition, sputtering, chemical plating (electroless plating, electrolytic plating), etc. Alternatively, the laminate may be one in which circuit processing is performed on these metal layers.

[0063] In sputtering or vapor deposition, a metal is sputtered or vapor-deposited to bring the metal parts into contact with each other and bond them together. Sputtering or vapor deposition is a well-known method in the field of electronic substrate manufacturing. Examples of metals for sputtering or vapor deposition include copper, aluminum, gold, tin, and chromium.

[0064] Electroless plating is a process in which a metal is deposited on a film from a solution containing metal ions, forming a bond between the two. Electroless plating is a well-known method in the field of manufacturing plated products on non-conductive materials (such as plastics and ceramics). Metals that can be used include copper, nickel, cobalt, gold, tin, and chromium.

[0065] The metal layer formed by sputtering, vapor deposition, electroless plating or the like may be thickened by electrolytic plating using the same or a different metal.

[0066] The thickness of the metal layer can be appropriately set depending on the application of the metal-clad laminate, and can be selected from a wide range of, for example, 10 nm to 100 μm. When a metal foil is used as the metal layer, the thickness of the metal layer may be 1 to 100 μm, preferably 5 to 50 μm, and more preferably 8 to 35 μm. When the metal layer is formed by sputtering, vapor deposition, electroless plating, or the like, or by a combination of these with electroplating, the thickness of the metal layer may be 10 nm to 35 μm, preferably 50 nm to 12 μm, and more preferably 100 nm to 9 μm.

[0067] The thermoplastic liquid crystal polymer film of the present invention is suitable for fine circuit processing by the semi-additive method, but does not prevent circuit formation by other methods, and may have a circuit drawn thereon using, for example, conductive ink. In particular, when the maximum valley depth Sv of the first surface is 0.2 μm or more and 2.0 μm or less, the film has excellent adhesiveness to conductive ink.

[0068] The pattern can be drawn using a conductive ink by, for example, drawing lines with a marker, drawing lines with an inkjet printer, or printing by screen printing, and is not particularly limited. Examples of conductive inks that can be used include water-based or oil-based inks containing metal particles such as Au, Pt, Ag, Cu, Ni, Cr, Rh, Pd, Zn, Co, Mo, Ru, W, Os, Ir, Fe, Mn, Ge, Sn, Ga, and In. After drawing with the conductive ink, it is preferable to perform a heat treatment to sinter the metal particles. Sintering can be performed at a temperature of approximately 180 to 450°C, but the heat treatment temperature is preferably lower than the melting point of the thermoplastic liquid crystal polymer film used as the substrate.

[0069] The laminate of the present invention may also have a metal foil pressure-bonded to the second surface by the above-mentioned method. Alternatively, a metal layer may be formed on the second surface by sputtering, vapor deposition, chemical plating, or the like. In this case, the surface roughness of the second surface may also be adjusted by the above-mentioned method so that the skewness Ssk is −5 or more and 0 or less.

[0070] The laminate of the present invention can be effectively used as a part used in the fields of electricity and electronics, office equipment and precision equipment, power semiconductors, etc., for example, as a circuit board material.

[0071] A circuit board using the laminate of the present invention is suitable for use as a high frequency circuit board, an in-vehicle sensor, a mobile circuit board, an antenna, and the like.

[0072] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the following examples and comparative examples, various physical properties were measured by the following methods.

[0073] [Thickness] The thickness of each material was measured using a Digimatic Indicator (manufactured by Mitutoyo Corporation). Measurements were taken across the width of the material at intervals of 1 cm, and the average value of 10 points randomly selected from the center and edge was recorded as the thickness.

[0074] [Melting Point] Using a differential scanning calorimeter (Shimadzu Corporation), a predetermined size sample was taken from the thermoplastic liquid crystal polymer film and placed in a sample container. The sample was heated from room temperature at a rate of 10°C / min until it was completely melted at 400°C. The melt was then cooled to 50°C at a rate of 10°C / min, and the temperature was raised again at a rate of 10°C / min. The position of the endothermic peak that appeared was determined as the melting point (Tm) of the thermoplastic liquid crystal polymer film.

[0075] [Measurement of Surface Roughness] The surface roughness of the thermoplastic liquid crystal polymer film was measured in accordance with ISO 25178 using a white light confocal microscope (OPTELICS HYBRID (L)) manufactured by Lasertec Corporation, measuring the arithmetic mean roughness Sa, maximum peak height Sp, maximum height Sz, deviation Ssk, and peak sharpness Sku. A 50x objective lens was used in the laser microscope, with a resolution of 0.05 μm and a measurement range of an area of ​​74.24 μm × 74.24 μm (5512 μm 2) was performed at three locations, the center and both sides, of a 30 cm wide sample, and the arithmetic mean values ​​of Sa, Sz, Ssk, and Sku at the three locations were defined as the values ​​of Sa, Sz, Ssk, and Sku. In the white light confocal microscope measurement, if the measurement surface was not flat but curved, flatness correction was performed before calculating the above surface properties. The measurement environment using the white light confocal microscope was a temperature of 23±2°C and a humidity of 50%±5%.

[0076] <Measurement of peel strength at copper layer / LCP film interface> A 5 ​​mm wide circuit was prepared from the copper vapor deposition layer of the laminate, and the thermoplastic liquid crystal polymer film was fixed to a flat plate with double-sided adhesive tape. The strength was measured when the copper foil was peeled off at a rate of 50 mm / min by the 90° method in accordance with JIS C 5016. The results in the table were converted into units from the sample width.

[0077] <Measurement of Transmission Loss and Impedance> After copper was vapor-deposited on the sample, the copper foil layer was plated up to 12 μm in a plating bath. A microstrip line structure was then formed. A circuit was fabricated so that the characteristic impedance was 50 Ω. For this circuit, the transmission loss and impedance were measured at 50 GHz using a microwave network analyzer (Agilent Technologies "8722ES") and a Cascade Microtec probe (ACP40-250). The transmission loss was measured immediately after the circuit board was left in an environment of 23°C temperature and 60% RH for 96 hours.

[0078] Example 1 A copolymer of p-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid (molar ratio: 80 / 20) was heated and kneaded at 280 to 340 ° C. using a single-screw extruder, and then extruded from an inflation die with a diameter of 40 mm and a slit spacing of 0.6 mm to obtain a thermoplastic liquid crystal polymer film having a thickness of 50 μm and a melting point of 320 ° C. Next, the heating temperature of a metal roll embossed with a surface roughness of Ra 0.9 μm, Rz 6.7 μm, and Rzjis 4.9 μm was set to 250 ° C., and the speed ratio of the metal roll peripheral speed to the film conveying speed was set to 0.98, and the thermoplastic liquid crystal polymer film was conveyed so that the holding time was 30 seconds, and the film was shrunk to obtain a film with a controlled surface shape (surface roughness). In the surface roughness of the embossed metal roll, Ra is the arithmetic mean roughness, Rz is the maximum height roughness, and Rzjis is the ten-point mean roughness, each of which is a value measured in accordance with JIS B 0601: 2001. The above-mentioned "holding time" refers to the time during which the thermoplastic liquid crystal polymer film is in contact with the metal roll surface in the process of conveying the film in contact with the metal roll surface.

[0079] Example 2 A thermoplastic liquid crystal polymer film having a controlled surface shape was obtained in the same manner as in Example 1, except that the ratio of the metal roll peripheral speed to the film conveying speed was 0.99 and the holding time was 10 seconds.

[0080] Example 3 In the same manner as in Example 1, a 50 μm thick thermoplastic liquid crystal polymer film was obtained by inflation film formation. On the other hand, the surface of a heat-resistant rubber roll was polished using 1200-grit rotary sandpaper to prepare a surface-roughened heat-resistant rubber roll. The thermoplastic liquid crystal polymer film was then placed on a copper foil (JX Nippon Mining Corporation: JXEFL-BHM foil, thickness 12 μm) and conveyed at a speed of 3 mm / m with the thermoplastic liquid crystal polymer film side in contact with and along the heat-resistant rubber roll. The film was introduced between the heat-resistant rubber roll and the heated metal roll for lamination and pressure bonding. At the same time, the roughened surface of the heat-resistant rubber roll was transferred onto the thermoplastic liquid crystal polymer film surface, resulting in a single-sided copper-clad laminate. The temperature of the heated metal roll was set to 240 ° C., and the pressure applied to the thermoplastic liquid crystal polymer film and copper foil during lamination and pressure bonding was 40 kg / cm in terms of surface pressure.2 was set to.

[0081] Example 4 A single-sided copper-clad laminate was obtained in the same manner as in Example 3, except that the laminate of the thermoplastic liquid crystal polymer film and the metal foil was moved along a heat-resistant rubber roll at a speed of 1 mm / min.

[0082] Comparative Example 1 A copolymer of p-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid (molar ratio: 80 / 20), melting point 320 ° C., was extruded from an extruder while pulling a vent and formed into a film using a T-die to obtain a 50 μm thick thermoplastic liquid crystal polymer film. The above thermoplastic liquid crystal polymer film and copper foil (JX Metals Corporation, JXEFL-BHM foil, 12 μm) were laminated, and further, polyimide films (Kaneka Corporation, "Apical" 50 μm) were placed on top and bottom as protective materials, and the surface temperature was set at 280 ° C. and the linear pressure was set at 4.2 kg / mm. The laminate was then cooled while being conveyed, and after cooling, the polyimide film was peeled off to obtain a single-sided copper-clad laminate consisting of copper foil and a smooth liquid crystal polymer film.

[0083] Comparative Example 2 In the same manner as in Example 1, a 50 μm thick thermoplastic liquid crystal polymer film was obtained by the inflation film forming method. Thereafter, a glossy heat-resistant rubber roll and a heated metal roll heated to 240 ° C were prepared, and the thermoplastic liquid crystal polymer film and copper foil (JX Nippon Mining Corporation: JXEFL-BHM foil, thickness 12 μm) were stacked together. The thermoplastic liquid crystal polymer film was then brought into contact with the heat-resistant rubber roll and conveyed at a speed of 2 mm / m along the heat-resistant rubber roll. The film was introduced between the heat-resistant rubber roll and the heated metal roll for lamination and pressure bonding. At the same time, the glossy side of the heat-resistant rubber roll was transferred onto the thermoplastic liquid crystal polymer film surface, and a single-sided copper-clad laminate was obtained. The pressure applied to the thermoplastic liquid crystal polymer film and copper foil during lamination and pressure bonding was 40 kg / cm in terms of surface pressure. 2 was set to.

[0084] Comparative Example 3 A single-sided copper-clad laminate was produced from a thermoplastic liquid crystal polymer film extruded from a T-die and copper foil in the same manner as in Comparative Example 1. Then, a solution of 30 wt% potassium hydroxide, 40 wt% monoethanolamine, and 30 wt% water at 90°C was prepared, and the thermoplastic liquid crystal polymer film surface was chemically etched by transporting the film so that the immersion time was 90 seconds.

[0085] Comparative Example 4 A thermoplastic liquid crystal polymer film having a thickness of 50 μm was obtained by the same inflation film forming method as in Example 1. Next, this thermoplastic liquid crystal polymer film and copper foil were laminated and pressure-bonded to produce a single-sided copper-clad laminate in the same manner as in Comparative Example 1. Thereafter, while this single-sided copper-clad laminate was conveyed at a conveying speed of 1 m / min, the surface of the thermoplastic liquid crystal polymer film was buffed at a high speed of 2000 rpm using a 1000 mesh buff roll with silicon carbide abrasive attached to nylon fibers.

[0086] Comparative Example 5 A 50 μm thick thermoplastic liquid crystal polymer film was obtained using the same inflation film forming method as in Example 1. Then, in the same manner as in Comparative Example 1, the inflation-formed thermoplastic liquid crystal polymer film and copper foil were laminated and pressure-bonded to produce a single-sided copper-clad laminate. The thermoplastic liquid crystal polymer film surface was then blasted using a wet blasting device. Polygonal alumina with an average particle size of 14 μm was used as the abrasive, and a mixture of the abrasive and water at a concentration of 15% by mass was sprayed using a wide gun. The spray pressure was 0.25 MPa. While performing blasting under the above conditions, the single-sided copper-clad laminate attached to the flat plate was transported at a transport speed of 50 mm / s, and the thermoplastic liquid crystal polymer film surface was blasted.

[0087] The surface roughness of the thermoplastic liquid crystal polymer film of the examples and comparative examples prepared as described above, or the surface of the thermoplastic liquid crystal polymer film of the single-sided copper-clad laminate, was measured by the method described above. The results are shown in Table 7. Next, a copper vapor-deposited layer was formed on the thermoplastic liquid crystal polymer film surface with the adjusted surface roughness by the following method.

[0088] <Formation of Copper Vapor Deposition Layer> Next, a roll-to-roll method using a vacuum deposition apparatus (manufactured by ROCK GIKEN KOGYO CO., LTD., product name: RVC-W-300) was employed to form a copper vapor deposition layer (thickness: 0.3 μm) on the thermoplastic liquid crystal polymer film or on the side surface of the thermoplastic liquid crystal polymer film in a single-sided copper-clad laminate.

[0089] More specifically, a thermoplastic liquid crystal polymer film or a single-sided copper-clad laminate was set on the loader side, the open window was completely closed, and then a vacuum was drawn. At the same time, the temperature of the heating roll (the roll on which metal is vapor-deposited onto the thermoplastic liquid crystal polymer film) was set to 100°C.

[0090] Next, the copper ingot was removed, and copper pellets were added so that the total weight of copper became 450 g. The copper pellets were pre-treated by washing with sodium persulfate water and then washed with distilled water.

[0091] Next, the vacuum level in the deposition chamber was 7×10 -3 After confirming that the vapor deposition pressure reached 100 Pa, the temperature of the heating roll was set to 280° C. Then, the output of the EMI (electron gun emission current value) was increased to melt the copper. At this time, the EMI output value was adjusted so that the deposition rate was 2.7 nm / s.

[0092] Next, the temperature of the heating roll reached the set temperature (280°C), and the vacuum level in the deposition chamber reached 5 x 10 -3 After confirming that the pressure was below 1 Pa, copper was vapor-deposited with the single-sided copper-clad laminate conveying speed set to 0.5 m / min to form a copper vapor-deposited layer with a thickness of 0.3 μm. The copper was then plated up to a thickness of 12 μm. The plating solution consisted of 100 g / L copper sulfate, 50 g / L sulfuric acid, 30 mg / L chloride ion concentration, and a small amount of additives. The plating current density was 1 A / dm 2 The temperature was set to 10° C., and electrolytic plating was carried out until a predetermined thickness was achieved.

[0093] The copper vapor-deposited layers formed in the examples and comparative examples were evaluated for peel strength and transmission characteristics using the methods described above. Peel strength was evaluated as good when it was 0.7 kN / m or higher, and transmission characteristics were evaluated as "good" when it was -8 dB / 100 mm or lower at 50 GHz, and "poor" when it was -8 dB / 100 mm or higher. The results are shown in Table 7.

[0094]

[0095] As shown in the table, Examples 1 to 4, in which the skewness Ssk and arithmetic mean roughness Sa fall within the range of the present invention, show good results in both peel strength and transmission characteristics. In contrast, Comparative Examples 1 and 2 have good transmission characteristics but low peel strength because the interface between the thermoplastic liquid crystal polymer film and the metal layer is flat, and Comparative Examples 3, 4, and 5, in which surface roughening outside the range of the present invention is applied, have high peel strength but poor transmission characteristics.

[0096] The thermoplastic liquid crystal polymer film of the present invention is suitable for forming fine circuits by a semi-additive method, and can achieve both peel strength and transmission properties, making it highly applicable to applications such as flexible circuit boards.

[0097] While the preferred embodiments of the present invention have been described above, those skilled in the art will readily recognize various changes and modifications within the scope of the present invention, which are obvious from the description of the present invention. Therefore, such changes and modifications are to be interpreted as falling within the scope of the invention as defined by the claims.

Claims

1. A thermoplastic liquid crystal polymer film containing a polymer capable of forming an optically anisotropic molten phase (hereinafter referred to as a thermoplastic liquid crystal polymer), in which the skewness (degree of bias) Ssk on at least one surface is -5 or more and 0 or less, and the arithmetic mean roughness Sa of the surface is 0.15 μm or more.

2. The thermoplastic liquid crystal polymer film of claim 1, wherein said surface is metal-free.

3. A thermoplastic liquid crystal polymer film according to claim 1 or 2, wherein the arithmetic mean roughness Sa of the surface is 0.5 μm or less.

4. A thermoplastic liquid crystal polymer film according to claim 1 or 2, wherein the maximum peak height Sp of the surface is 0.15 or more and 3.00 or less.

5. A thermoplastic liquid crystal polymer film according to claim 1 or 2, wherein the maximum valley depth Sv of the surface is 0.2 μm or more and 3.5 μm or less.

6. A thermoplastic liquid crystal polymer film according to claim 1 or 2, wherein the maximum height Sz of the surface is 1.5 μm or more and 5.0 μm or less.

7. A thermoplastic liquid crystal polymer film according to claim 1 or 2, having a melting point of 315°C or higher.

8. A laminate comprising the thermoplastic liquid crystal polymer film according to claim 1 or 2 and a conductive layer laminated on the thermoplastic liquid crystal polymer film.

9. A laminate according to claim 8, in which a conductive layer is formed on the surface of the thermoplastic liquid crystal polymer film, the conductive layer being composed of at least one material selected from the group consisting of conductive ink, metal film, and circuits formed therefrom.

10. The laminate according to claim 9, wherein a metal foil layer is formed as a conductive layer on the surface opposite to the surface of the thermoplastic liquid crystal polymer film.

11. The laminate of claim 8, which is a circuit board.

12. A method for producing a thermoplastic liquid crystal polymer film according to claim 1 or 2, comprising at least a step of contacting at least one surface of the thermoplastic liquid crystal polymer film with a roll having a roughened surface.

13. A method for producing a laminate according to claim 8, comprising at least a step of contacting a surface of the thermoplastic liquid crystal polymer film of a laminate of a thermoplastic liquid crystal polymer film and a support with a roll having a roughened surface.

14. The method for producing a laminate according to claim 13, wherein the support is a metal foil.

Citation Information

Patent Citations

  • Method for manufacturing metal-clad laminated sheet

    JP2002331589A

  • Resin sheet and resin laminate substrate

    JP2019104157A

  • Printed wiring board substrate, printed wiring board, manufacturing method of printed wiring board substrate, and manufacturing method of printed wiring board

    JP2020057799A

  • Polypropylene film, metal membrane layered film using same, and film capacitor

    WO2021166994A1

  • Thermoplastic liquid crystal polymer molded article

    WO2021251261A1