Curable composition, sealant, frame sealant, display panel and method for producing same

The curable composition, featuring a cationic photopolymerization initiator, tertiary amine, and inorganic filler, addresses the challenges of high-temperature curing and viscosity increase in sealants for organic EL display panels by maintaining low viscosity and ensuring high adhesive strength, enhancing the sealing process's effectiveness.

WO2024204248A1PCT designated stage expired Publication Date: 2024-10-03MITSUI CHEMICALS INC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012039
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-26
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing sealants for organic electroluminescent (EL) display panels face challenges with high-temperature curing, leading to damage of elements, and excessive viscosity increase after light irradiation, which impairs fluidity and tack, making it difficult to achieve both low-temperature curability and sufficient adhesive strength.

Method used

A curable composition comprising a cationic photopolymerization initiator, a tertiary amine, and an inorganic filler, where the tertiary amine content is optimized to trap acid generated during light irradiation, maintaining low viscosity and allowing for low-temperature curing, thereby preventing excessive viscosity increase and ensuring high adhesive strength.

Benefits of technology

The curable composition achieves low-temperature curability while maintaining low viscosity after light irradiation, resulting in a sealant with improved moisture barrier properties and high adhesive strength, reducing the risk of element damage during the sealing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

This curable composition contains a curable compound, a photocationic polymerization initiator, a tertiary amine, and an inorganic filler. The content of the tertiary amine is 20 parts by mass or more relative to 100 parts by mass of the photocationic polymerization initiator.
Need to check novelty before this filing date? Find Prior Art

Description

Curable composition, sealant, frame sealant, display panel, and method for producing the same

[0001] The present invention relates to a curable composition, a sealant, a frame sealant, a display panel, and a method for producing the same.

[0002] In recent years, display devices using display elements such as organic electroluminescence elements (hereinafter referred to as organic EL elements) have been developed, but display elements are generally susceptible to deterioration due to moisture and oxygen in the atmosphere. Therefore, in various display devices, the display elements are generally sealed with a sealing layer.

[0003] For example, an organic EL display panel includes an element substrate having organic EL elements, an opposing substrate, and a sealing layer disposed between them to seal the organic EL elements. Such organic EL display panels are manufactured by various methods. One such manufacturing method is known as the dam-fill method.

[0004] In the dam-fill method, an organic EL display panel is manufactured through, for example, 1) a step of applying a first sealant in a frame shape onto an opposing substrate, 2) a step of filling a second sealant into the area surrounded by the first sealant to form a sealant layer, 3) a step of irradiating the sealant layer with light, 4) a step of bonding a substrate on which an organic EL element is disposed to the opposing substrate having the sealant layer after light irradiation, and 5) a step of heating and curing the sealant layer (see, for example, Patent Document 1).

[0005] Furthermore, as a frame sealant used in the above-mentioned method, for example, a sealant containing a polyolefin, an epoxy compound (curable resin A), a thermosetting agent, and a water-absorbing filler is known (see, for example, Patent Document 2). In this document, a thermal cationic initiator is used as the thermosetting agent.

[0006] Further, as a sealant for an organic EL element, a sealant containing a photocurable compound containing a (meth)acrylic-modified epoxy resin and a photocationic polymerization initiator is also known (see, for example, Patent Document 3).

[0007] International Publication No. 2013 / 157059 International Publication No. 2020 / 149359 Japanese Patent Application Laid-Open No. 2012-151109

[0008] However, the sealant disclosed in Patent Document 2 has a problem in that the element is easily damaged by heating because it is cured by heating at 100° C. In order to prevent such damage, the sealant is required to have low-temperature curing properties.

[0009] Furthermore, the above-described sealant is required to have a predetermined usable time or more after light irradiation, i.e., to maintain a moderately low viscosity after light irradiation. For example, as described above, the sealant applied to one substrate is irradiated with light to temporarily cure, and then the other substrate is bonded to the substrate and heated to fully cure. However, the sealants shown in Patent Documents 2 and 3 tend to undergo an excessive increase in viscosity after light irradiation because the curing reaction proceeds too quickly before the other substrate is bonded. As a result, there is a problem in that the fluidity and tack of the sealant are easily impaired during bonding, making it difficult to obtain sufficient adhesive strength. Generally, the higher the low-temperature curing property, the more likely the viscosity is to increase after light irradiation, so it is desirable to achieve a good balance between these properties.

[0010] Furthermore, the frame sealant that seals the periphery of the element contains a filler to reduce the moisture permeability of the cured product and improve its shape retention. Such sealants exhibit a greater increase in viscosity after light irradiation, making them more susceptible to loss of fluidity and tack during lamination. Therefore, it is even more important to maintain a low viscosity after light irradiation.

[0011] The present invention has been made in view of the above circumstances, and provides a curable composition that combines low-temperature curing properties and viscosity stability after light irradiation and is capable of providing a cured product that has low moisture permeability and high adhesive strength, a sealant, a frame sealant, a display panel, and a method for producing the same.

[0012] [1] A curable composition comprising a curable compound, a photocationic polymerization initiator, a tertiary amine, and an inorganic filler, wherein the content of the tertiary amine is 20 parts by mass or more relative to 100 parts by mass of the photocationic polymerization initiator. [2] The curable composition according to [1], wherein the content of the tertiary amine is 0.5 parts by mass or more and 20 parts by mass or less relative to 100 parts by mass of the curable compound. [3] The curable composition according to [1] or [2], wherein the content of the inorganic filler is 20 parts by mass or more and 400 parts by mass or less relative to 100 parts by mass of the curable compound. [4] The curable composition according to any one of [1] to [3], wherein the curable compound includes an aromatic epoxy compound. [5] The curable composition according to any one of [1] to [4], wherein the tertiary amine is a bifunctional tertiary amine. [6] The curable composition according to any one of [1] to [5], wherein the tertiary amine has an N—O bond. [7] The curable composition according to any one of [1] to [6], wherein the tertiary amine has a hindered structure. [8] The curable composition according to any one of [1] to [6], wherein the curable composition is irradiated with light having a wavelength of 365 nm at a UV irradiance of 100 mW / cm. 2 The cumulative light intensity is 3000 mJ / cm 2 The viscosity at 25°C 60 seconds after irradiation was 1.0 x 10 4

[10] A frame sealant comprising the curable composition according to any one of [1] to [8].

[11] A display panel comprising: an element substrate on which elements are arranged; a counter substrate arranged opposite the element substrate with the elements interposed therebetween; and a sealing portion arranged between the element substrate and the counter substrate for sealing the elements, wherein the sealing portion comprises a cured product of the sealant according to [9].

[12] A method for manufacturing a display panel, comprising the steps of: applying a first sealant in a frame shape along the periphery of a display area on one surface of an element substrate or an opposing substrate, filling the area surrounded by the first sealant with a second sealant to form a sealant layer, irradiating the sealant layer with light, bonding one substrate to the other substrate via the sealant layer irradiated with light, and heating and curing the sealant layer, wherein at least one of the first sealant and the second sealant is the sealant described in [9].

[13] A method for manufacturing a display panel, according to

[12] , wherein the first sealant is the sealant described in [9].

[0013] The present invention has been made in view of the above circumstances, and provides a curable composition that combines low-temperature curing properties and viscosity stability after light irradiation and is capable of providing a cured product that has low moisture permeability and high adhesive strength, a sealant, a frame sealant, a display panel, and a method for producing the same.

[0014] As described above, curable compositions having low-temperature curing properties tend to increase in viscosity after light irradiation and are unable to maintain a low viscosity.

[0015] In contrast, the curable composition of the present invention contains a curable compound, a photocationic polymerization initiator, a tertiary amine, and an inorganic filler. The content of the tertiary amine in the curable composition of the present invention is a predetermined amount or more relative to the amount of the photocationic polymerization initiator. This allows the composition to achieve both low-temperature curability and viscosity stability after light irradiation, even when the composition contains an inorganic filler. The mechanism behind this is unclear, but is presumed to be as follows.

[0016] When the curable composition is first irradiated with light, an acid is generated from the photocationic polymerization initiator. This acid is captured by a sufficient amount of tertiary amine. Therefore, at the time of light irradiation, curing of the curable compound is slow, and the viscosity of the curable composition after light irradiation is maintained low. When the curable composition is then heated at a low temperature, the acid captured by the tertiary amine is released, and the curable compound is cured. Therefore, this curable composition has excellent low-temperature curing properties. As a result, when this curable composition is used to seal optical elements in, for example, a display panel equipped with optical elements, it can seal the optical elements with low moisture permeability and high adhesive strength while suppressing thermal damage to the optical elements. A curable composition according to one embodiment of the present invention will now be described in detail.

[0017] 1. Curable Composition The curable composition according to this embodiment contains a curable compound, a photocationic polymerization initiator, a tertiary amine, and an inorganic filler.

[0018] 1-1. Curable Compound The curable compound includes a curable compound that polymerizes and cures due to active species generated from a photocationic polymerization initiator. Examples of such curable compounds include epoxy compounds and oxetane compounds, but from the viewpoint of enhancing thermosetting properties, it is preferable to include an epoxy compound. The curable compound may include only one type of epoxy compound, or may include two or more types.

[0019] In this specification, an epoxy compound refers to a compound having one or more epoxy groups in the molecule. The number of epoxy groups contained in one molecule of the epoxy compound may be one or two or more. From the viewpoint of increasing the curing reactivity, the number of epoxy groups contained in one molecule of the epoxy compound is preferably two or more.

[0020] Examples of the epoxy compound include known epoxy compounds, such as aromatic epoxy compounds, aliphatic epoxy compounds, and alicyclic epoxy compounds. Among these, from the viewpoint of further reducing the moisture permeability of the cured product, it is preferable that at least one of the epoxy compounds includes an aromatic epoxy compound.

[0021] Examples of aromatic epoxy compounds include glycidyl ethers of alcohols (including polyhydric alcohols) containing an aromatic ring. Specific examples include bisphenol-type glycidyl ether compounds obtained by reacting epichlorohydrin with bisphenols such as bisphenol A, bisphenol S, bisphenol F, and bisphenol AD, or diols obtained by modifying these aromatic diols with ethylene glycol, propylene glycol, and alkylene glycol; trisphenol-type glycidyl ether compounds obtained by reacting epichlorohydrin with trisphenol compounds (e.g., 1,1,1-tris(hydroxyphenyl)methane, 1-[α-methyl-α-(4-hydroxyphenyl)ethyl]-3-[α,α-bis(4-hydroxyphenyl)ethyl]benzene (or 4-[4-[1,1-bis(4-hydroxyphenyl)ethyl]-α,α-dimethylbenzyl]phenol); These include novolak resins derived from phenol or cresol and formaldehyde, novolak-type glycidyl ether compounds obtained by reacting polyphenols, such as polyalkenylphenols or their copolymers, with epichlorohydrin, and glycidyl ether compounds of xylylene phenol resins.

[0022] Among these, bisphenol-type epoxy compounds such as bisphenol A-type epoxy compounds and bisphenol F-type epoxy compounds, cresol novolac-type epoxy compounds, phenol novolac-type epoxy compounds, triphenolmethane-type epoxy compounds, triphenolethane-type epoxy compounds, trisphenol-type epoxy compounds, dicyclopentadiene-type epoxy compounds, diphenyl ether-type epoxy compounds, and biphenyl-type epoxy compounds are preferred.

[0023] The epoxy compound may be liquid or solid. From the viewpoint of improving the coatability of the curable composition, a liquid epoxy compound is preferred. Furthermore, from the viewpoint of further reducing the moisture permeability of the cured product, a solid epoxy compound is preferred. The softening point of the solid epoxy compound is preferably 40°C or higher and 150°C or lower. The softening point can be measured by the ring and ball method specified in JIS K7234.

[0024] The weight average molecular weight of the epoxy compound is preferably from 200 to 10,000, and more preferably from 300 to 5,000. The weight average molecular weight of the epoxy compound is measured by gel permeation chromatography (GPC) in terms of polystyrene.

[0025] As described above, the curable compound may contain only one type of epoxy compound, or may contain two or more types. For example, from the viewpoint of achieving both viscosity stability and permeability of the cured product at a higher level, a liquid epoxy compound and a solid epoxy compound may be combined. Furthermore, from the viewpoint of easily achieving both viscosity stability and permeability of the cured product, a bifunctional aromatic epoxy compound and a trifunctional or higher aromatic epoxy compound may be combined.

[0026] For example, when a difunctional aromatic epoxy compound is combined with a trifunctional or higher aromatic epoxy compound, the trifunctional or higher aromatic epoxy compound can be, for example, 10% by mass or more, preferably 30% by mass or more and 70% by mass or less, based on the total amount of epoxy compounds. When the content of the trifunctional or higher aromatic epoxy compound is 10% by mass or more, the moisture permeability of the cured product can be further improved. On the other hand, although the viscosity of the curable composition after light irradiation tends to increase, the tertiary amine traps the acid generated from the photocationic polymerization initiator, thereby suppressing excessive viscosity increase.

[0027] The curable compound may also include both an epoxy compound and an oxetane compound.

[0028] The content of the epoxy compound is preferably 30% by mass or more, more preferably 50% by mass or more, and may be 100% by mass, based on the curable compound. When the amount of the epoxy compound is 30% by mass or more, the curing reactivity by heating is more likely to be increased.

[0029] The total amount of the curable compounds is preferably 20% by mass or more and 90% by mass or less, and more preferably 30% by mass or more and 70% by mass or less, relative to the curable composition. When the amount of the curable compounds is 20% by mass or more, curing reactivity is more easily obtained, and the adhesive strength of the cured product is more easily increased. On the other hand, when the amount of the curable compounds is 90% by mass or less, for example, the amount of inorganic filler becomes relatively large, and the shape retention of the resulting sealant is more easily improved.

[0030] 1-2. Photocationic Polymerization Initiator The photocationic polymerization initiator is, for example, a photoacid generator that generates an acid upon irradiation with light.

[0031] The absorption wavelength of the cationic photopolymerization initiator is not particularly limited, and it is preferable that the initiator absorbs light having a wavelength of 360 nm or more, and more preferably absorbs light having a wavelength of 360 nm or more and 430 nm or less. When the absorption wavelength of the cationic photopolymerization initiator is within the above range, it is possible to reduce the influence on optical elements, for example.

[0032] The cationic photopolymerization initiator is not particularly limited, and known cationic photopolymerization initiators can be used.

[0033] Examples of photocationic polymerization initiators include those in which the anion moiety is BF 4 - , (Rf) n PF 6-n - (Rf is an organic group, n is an integer of 1 to 5), PF 6 - , SbF 6 - , or BX 4 - (X is a phenyl group substituted with at least two fluorine atoms or trifluoromethyl groups), aromatic sulfonium salts, aromatic iodonium salts, aromatic diazonium salts, aromatic ammonium salts, etc. are included.

[0034] Examples of the aromatic sulfonium salt include bis[4-(diphenylsulfonio)phenyl]sulfide bishexafluorophosphate, bis[4-(diphenylsulfonio)phenyl]sulfide bishexafluoroantimonate, bis[4-(diphenylsulfonio)phenyl]sulfide bistetrafluoroborate, bis[4-(diphenylsulfonio)phenyl]sulfide tetrakis(pentafluorophenyl)borate, diphenyl-4-(phenylthio)phenylsulfonium hexafluorophosphate, diphenyl-4-(phenylthio)phenylsulfonium hexafluoroantimonate, diphenyl-4-(phenylthio)phenylsulfonium tetrafluoroborate, and the like.

[0035] Examples of aromatic iodonium salts include diphenyliodonium hexafluorophosphate, diphenyliodonium hexafluoroantimonate, diphenyliodonium tetrafluoroborate, diphenyliodonium tetrakis(pentafluorophenyl)borate, bis(dodecylphenyl)iodonium hexafluorophosphate, bis(dodecylphenyl)iodonium hexafluoroantimonate, bis(dodecylphenyl)iodonium tetrafluoroborate, bis(dodecylphenyl)iodonium tetrakis(pentafluorophenyl)borate, and the like.

[0036] Examples of aromatic diazonium salts include phenyldiazonium hexafluorophosphate, phenyldiazonium hexafluoroantimonate, phenyldiazonium tetrafluoroborate, phenyldiazonium tetrakis(pentafluorophenyl)borate, and the like.

[0037] Examples of aromatic ammonium salts include 1-benzyl-2-cyanopyridinium hexafluorophosphate, 1-benzyl-2-cyanopyridinium hexafluoroantimonate, and the like.

[0038] Examples of commercially available photocationic polymerization initiators include Irgacure 250, Irgacure 270, and Irgacure 290 (manufactured by BASF), CPI-100P, CPI-101A, CPI-200K, CPI-210S, CPI-310B, and CPI-400PG (manufactured by San-Apro Co., Ltd.), and SP-150, SP-170, SP-171, SP-056, SP-066, SP-130, SP-140, SP-601, SP-606, and SP-701 (manufactured by ADEKA Corporation). Of these, sulfonium salts such as Irgacure 270, Irgacure 290, CPI-100P, CPI-101A, CPI-200K, CPI-210S, CPI-310B, CPI-400PG, SP-150, SP-170, SP-171, SP-056, SP-066, SP-601, SP-606, and SP-701 are preferred.

[0039] The cationic photopolymerization initiator may be used alone or in combination of two or more kinds.

[0040] The content of the cationic photopolymerization initiator is preferably 0.1 parts by mass or more and 20 parts by mass or less, more preferably 0.5 parts by mass or more and 15 parts by mass or less, and even more preferably 0.8 parts by mass or more and 8 parts by mass or less, relative to 100 parts by mass of the curable compound. When the content of the cationic photopolymerization initiator is 0.1 parts by mass or more, a larger amount of acid is more likely to be generated by light irradiation, which can make the curing reaction more likely to occur when curing by heating. When the content of the cationic photopolymerization initiator is 20 parts by mass or less, bleed-out can be reduced, which can reduce contamination of optical elements and the like.

[0041] Tertiary amines capture the acid generated from the cationic photopolymerization initiator upon light irradiation, thereby making it difficult for the curing reaction of the curable compound to occur upon light irradiation and suppressing an excessive increase in viscosity of the curable composition after light irradiation.

[0042] Tertiary amines include monofunctional tertiary amines having one amino group in the molecule, bifunctional tertiary amines having two amino groups, and trifunctional or higher tertiary amines having three or more amino groups. Among these, from the viewpoint of further increasing the acid trapping efficiency, bifunctional tertiary amines and trifunctional or higher tertiary amines are preferred, and from the viewpoint of more easily maintaining compatibility with the epoxy compound, bifunctional tertiary amines are more preferred.

[0043] The tertiary amine preferably has an N—O bond, from the viewpoint of making it easier to release the trapped acid upon heating and further improving low-temperature curing properties. In other words, a bifunctional tertiary amine having an N—O bond is preferred.

[0044] Furthermore, the tertiary amine preferably has a hindered structure, which makes it easier to release the trapped acid upon heating and further enhances low-temperature curing properties. Examples of the hindered structure include a structure having a steric hindrance, such as 2,2,6,6-tetramethylpiperidine.

[0045] Therefore, the tertiary amine is preferably a bifunctional tertiary amine having an N—O bond, more preferably a bifunctional tertiary amine having an N—O bond and a hindered structure, and even more preferably a tertiary amine having an N—O bond and two 2,2,6,6-tetramethylpiperidine structures in the molecule.

[0046] Such tertiary amines include compounds represented by formula (1) or (2).

[0047] In formula (1), R 3 represents an alkyl group having 1 to 20 carbon atoms. Examples of linear or branched alkyl groups having 1 to 20 carbon atoms include a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, an undecyl group, and an eicosyl group. 3 may be the same as or different from each other.

[0048]

[0049] In formula (2), R4 represents a linear or branched alkyl group having 1 to 20 carbon atoms. Examples of linear or branched alkyl groups having 4 to 20 carbon atoms include a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, an undecyl group, and an eicosyl group. 4 may be the same as or different from each other.

[0050] R 5 represents an alkylene group having 1 to 8 carbon atoms. Examples of the alkylene group having 1 to 8 carbon atoms include a methylene group, an ethylene group, a propylene group, a butylene group, a pentylene group, a hexylene group, a heptylene group, and an octylene group.

[0051] Examples of the compound represented by formula (1) include a compound represented by formula (1-1); examples of the compound represented by formula (2) include a compound represented by formula (2-1).

[0052] Commercially available tertiary amines may also be used, such as ADK STAB LA-81 (manufactured by ADEKA Corporation) and Tinuvin 123 (manufactured by BASF Japan).

[0053] The tertiary amine may be contained in one kind or in two or more kinds.

[0054] The content of the tertiary amine is preferably 20 parts by mass or more per 100 parts by mass of the cationic photopolymerization initiator from the viewpoint of capturing the acid generated from the cationic photopolymerization initiator. When the content of the tertiary amine is 20 parts by mass or more, a large amount of acid can be trapped, which makes it easier to suppress an increase in viscosity after light irradiation and further enhances tackiness. From the same viewpoint, the content of the tertiary amine is preferably 60 parts by mass or more, more preferably 65 parts by mass or more, per 100 parts by mass of the cationic photopolymerization initiator. The upper limit of the content of the tertiary amine is not particularly limited, but may be, for example, 100 parts by mass or less from the viewpoint of further reducing the amount of tertiary amine remaining as an unreacted component after curing, further minimizing deterioration in the adhesion and moisture permeability of the cured product, and improving the physical properties of the cured product.

[0055] Furthermore, the content of the tertiary amine is, for example, preferably 0.5 parts by mass or more and 20 parts by mass or less, and more preferably 1 part by mass or more and 5 parts by mass or less, relative to 100 parts by mass of the curable compound. When the content of the tertiary amine is 0.5 parts by mass or more, a larger amount of acid can be trapped, making it easier to suppress an increase in viscosity after light irradiation and further increasing tack. When the content of the tertiary amine is 20 parts by mass or less, the amount of tertiary amine remaining unreacted after heat curing can be further reduced, making it possible to further suppress deterioration in the physical properties of the cured product.

[0056] 1-4. Inorganic Filler The inorganic filler can have the function of improving the shape retention of the curable composition and reducing the moisture permeability of the cured product.

[0057] Examples of inorganic fillers include calcium carbonate, magnesium carbonate, barium sulfate, magnesium sulfate, aluminum silicate, zirconium silicate, iron oxide, titanium oxide, titanium nitride, alumina other than those mentioned above, zinc oxide, silicon dioxide (silica), potassium titanate, kaolin, talc, glass beads, sericite activated clay, bentonite, aluminum nitride, silicon nitride, etc. Of these, silicon dioxide and talc are preferred.

[0058] The inorganic filler may have a regular shape, such as a spherical, plate-like, or needle-like shape, or may have an irregular shape. When the inorganic filler is spherical, the average primary particle diameter of the inorganic filler is preferably 0.1 μm or more and 5 μm or less, and more preferably 0.5 μm or more and 3 μm or less, from the viewpoints of, for example, the shape retention and thickness adjustment of the cured product after lamination and reducing the moisture permeability. When the average primary particle diameter of the inorganic filler is 5 μm or less, thickness unevenness of the cured product after lamination can be more easily reduced, and when it is 0.1 μm or more, an increase in viscosity can be further suppressed. Furthermore, from the viewpoint of adjusting the viscosity (thixotropy) of the curable composition, the average primary particle diameter is preferably in the range of less than 0.1 μm, for example, 7 nm or more and less than 100 nm. The average primary particle diameter of the inorganic filler can be measured by the laser diffraction method described in JIS Z8825 (2013).

[0059] The specific surface area of ​​the inorganic filler is 0.5 m 2 / g or more 20m 2 The specific surface area of ​​the inorganic filler is measured by the BET method described in JIS Z8830 (2013).

[0060] The curable composition may contain only one type of inorganic filler, or may contain two or more types. From the viewpoint of adjusting the viscosity (thixotropy) and the shape retention and thickness of the cured product, for example, the curable composition may contain an inorganic filler having a relatively small average primary particle size (e.g., less than 0.1 μm) and an inorganic filler having a relatively large average primary particle size (e.g., 0.1 μm or more). The content of the inorganic filler having a relatively small average particle size is preferably less than the content of the inorganic filler having a relatively large average particle size.

[0061] The content of the inorganic filler is preferably 10 parts by mass or more and 350 parts by mass or less relative to 100 parts by mass of the curable compound. When the content of the inorganic filler is 10 parts by mass or more, the shape retention of the cured product is more likely to be improved and moisture permeability can be further reduced. When the content of the inorganic filler is 350 parts by mass or less, not only is the coatability of the curable composition less likely to be impaired, but also a decrease in adhesive strength due to a decrease in the relative amount of the curable compound or a loss in flexibility of the cured product can be more suppressed. From the same viewpoint, the content of the inorganic filler is more preferably 150 parts by mass or more and 300 parts by mass or less.

[0062] 1-5. Others The curable composition may further contain other components in addition to the above-described components. Examples of the other components include a photosensitizer, a silane coupling agent, a tackifier, organic fine particles, a plasticizer, an antioxidant, and an antifoaming agent.

[0063] 1-5-1. Photosensitizer The photosensitizer has the function of further improving the polymerization initiation efficiency of the above-mentioned cationic photopolymerization initiator and further accelerating the curing reaction of the curable compound.

[0064] Examples of the photosensitizer include thioxanthone compounds such as 2,4-diethylthioxanthone, 2,2-dimethoxy-1,2-diphenylethan-1-one, benzophenone, 2,4-dichlorobenzophenone, methyl o-benzoylbenzoate, 4,4'-bis(dimethylamino)benzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, 9,10-dibutoxyanthracene, etc. The curable composition may contain only one type of photosensitizer, or may contain two or more types.

[0065] The content of the photosensitizer is, for example, preferably 0.1 parts by mass or more and 5 parts by mass or less, and more preferably 0.5 parts by mass or more and 2 parts by mass or less, relative to 100 parts by mass of the curable compound. The curable composition may contain only one type of photosensitizer, or may contain two or more types of photosensitizers.

[0066] 1-5-2. Silane Coupling Agent Examples of the silane coupling agent include vinyltrimethoxysilane, γ-(meth)acryloxypropyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, and γ-glycidoxypropyltriethoxysilane.

[0067] The content of the silane coupling agent is preferably 0.1 to 10 parts by mass, more preferably 1.0 to 5.0 parts by mass, relative to 100 parts by mass of the curable compound. When the content of the silane coupling agent is 0.1 part by mass or more, the adhesive strength of the cured product is more likely to be increased, and when it is 10 parts by mass or less, the decrease in moisture permeation resistance of the cured product can be further reduced.

[0068] 1-5-3. Common Features The total amount of the other components is preferably 0.1% by mass or more and 50% by mass or less, based on the total amount of the curable composition. When the total amount is 50% by mass or less, the viscosity of the curable composition is unlikely to increase excessively, and the coatability is unlikely to be impaired.

[0069] 1-6. Physical Properties The viscosity of the curable composition, measured using an E-type viscometer at 25°C and 2.5 revolutions per minute, is preferably, for example, 50 Pa·s or more and 400 Pa·s or less, and more preferably 100 Pa·s or more and 300 Pa·s or less. When the viscosity of the curable composition is 50 Pa·s or more, the composition has a moderately high viscosity, which makes it easier to improve shape retention during application. When the viscosity of the curable composition is 400 Pa·s or less, the application properties are less likely to be impaired when the composition is applied, for example, with a dispenser.

[0070] The curable composition was irradiated with light of 365 nm wavelength at an illuminance of 100 mW / cm 2 The cumulative light intensity is 3000 mJ / cm 2 After irradiation, the viscosity at 25°C 60 seconds later was 1.0 x 10 4 It is preferable that the viscosity is 1.0×10 Pa·s or less. 2 Pa・s or more 5.0×10 3 It is more preferable that the viscosity of the curable composition is 1.0×10 Pa s or less. 4 When the viscosity of the curable composition is 1.0×10 Pa s or less, the curable composition has tack even after light irradiation, and the fluidity at the time of lamination is less likely to be impaired, and the adhesive strength of the cured product can be increased. 2 When the viscosity is Pa·s or more, the curable composition after light irradiation can have better shape retention.

[0071] The viscosity after light irradiation is also measured using an E-type viscometer at 25°C and 2.5 revolutions per minute. Specifically, a 10 μm thick coating film of the curable composition is formed on a 0.7 mm thick alkali-free glass plate using a No. 6 bar coater. This coating film is left at room temperature (25°C) for 3 minutes while purging with nitrogen. Thereafter, ultraviolet light is applied to this coating film using a metal halide lamp with a wavelength of 365 nm at a UV irradiance of 100 mW / cm. 2 The cumulative light intensity is 3000 mJ / cm 2 After irradiation, the coating film is scraped off, and the viscosity after 60 seconds is measured in the same manner as above.

[0072] The viscosity of the curable composition after light irradiation can be adjusted by the content of the tertiary amine and the content of the inorganic filler. For example, if the amount of the tertiary amine is large relative to the amount of the cationic photopolymerization initiator, a larger amount of acid generated from the cationic photopolymerization initiator upon light irradiation can be trapped, which tends to reduce the increase in viscosity of the curable composition after light irradiation. On the other hand, the larger the content of the inorganic filler, the larger the increase in viscosity after light irradiation tends to be.

[0073] As described above, the curable composition according to this embodiment can be used as a sealant because its viscosity can be adjusted to a level suitable for bonding after light irradiation. That is, the sealant contains the curable composition.

[0074] As described below, the sealant can be used as a sealant or adhesive for various elements such as organic EL elements, LED elements, liquid crystal elements, semiconductor elements, and solar cell elements. For example, the sealant may be a sealant for sealing light-emitting elements such as organic EL elements and micro LED elements. The sealant may be a surface sealant or a frame sealant. Since the frame sealant is required to have a cured product with high shape retention, the curable composition is particularly suitable as a frame sealant.

[0075] Hereinafter, an example in which the curable composition is used as a sealant for a display panel will be described.

[0076] 2. Display Panel and Manufacturing Method Thereof A display panel according to one embodiment of the present invention has an element substrate, an opposing substrate, and a sealing portion disposed between them to seal the elements.

[0077] The element substrate includes a substrate and an element. The substrate is a transparent substrate. The material of the transparent substrate may be an inorganic material such as glass, or may be a plastic such as polycarbonate, polyethylene terephthalate, polyethersulfone, or PMMA. The element may be any of various elements such as an organic EL element, an LED element (including a micro LED), a liquid crystal element, a semiconductor element, or a solar cell element. For example, when the element is an organic EL element, the organic EL element is disposed on a substrate and has a laminated structure of an anode / light-emitting layer / negative electrode.

[0078] The counter substrate is disposed opposite the element substrate with the elements interposed therebetween. The counter substrate may be a transparent substrate similar to the above. The counter substrate may have, for example, a color filter layer.

[0079] The sealing portion includes a frame-shaped first sealing portion arranged to surround the outer periphery of the element, and a second sealing portion filled in the area surrounded by the first sealing portion. The first sealing portion is a cured product of a first sealant (dam material). The second sealing portion is a cured product of a second sealant (fill material). At least one of the first sealant and the second sealant, preferably the first sealant, is the curable composition.

[0080] The display panel can be manufactured by any method. For example, the display panel can be obtained by a manufacturing method including the steps of: 1) applying a first sealant in a frame shape on one of the counter substrate and the element substrate so as to surround a display region; 2) filling the region surrounded by the frame-shaped applied first sealant with a second sealant to form a sealant layer; 3) irradiating the sealant layer with light; 4) bonding the one substrate and the other substrate together via the sealant layer irradiated with light; and 5) heating and curing the sealant layer.

[0081] In step 1), the first sealant is applied to one of the opposing substrate and the element substrate, for example, the opposing substrate, in a frame shape so as to surround the display area. The application method is not particularly limited, but application can be performed using a dispenser, for example.

[0082] In step 2), a second sealant is filled into the area surrounded by the first sealant applied in a frame shape, thereby forming a sealant layer.

[0083] In step 3), the sealant layer is irradiated with light. The type of light to be irradiated is appropriately selected depending on the type of cationic photopolymerization initiator in the curable composition serving as the first sealant, but light in the visible light range is preferred, for example, light with a wavelength of 370 nm or more and 450 nm or less. This is because light in this wavelength range causes relatively little damage to the drive electrode. For the light irradiation, a known light source emitting ultraviolet or visible light can be used, such as a metal halide lamp.

[0084] The light irradiation amount is preferably such that the curable composition after irradiation remains adequately tacky. For example, 10 mW / cm 2 More than 1000mW / cm 2 At an intensity of 1000 mJ / cm 2 More than 10000mJ / cm 2 It can be as follows:

[0085] The light irradiation initiates curing of the first sealant and the second sealant. After the light irradiation is completed, the temperature of the substrate may rise to about 35°C, and the substrate may be left in this state. By waiting for a predetermined time after the light irradiation rather than immediately bonding the substrates, the curing of the first sealant and the second sealant progresses appropriately and the viscosity of the first sealant and the second sealant increases.

[0086] In step 4), in a state in which the viscosities of the first sealant and the second sealant have been appropriately increased, the opposing substrate and the element substrate are bonded together via the sealant layer.

[0087] The bonding is performed by pressing the element substrate and the opposing substrate with a press or the like in a vacuum chamber so as to crush the sealant layer. At this time, the first sealant, which has a relatively high viscosity, is present in a frame shape around the second sealant, preventing the second sealant from leaking out.

[0088] In step 5), the laminated body is heated to heat and harden the first sealant and the second sealant.

[0089] The heating temperature may be any temperature at which the sealant layer is cured, and from the viewpoint of reducing thermal damage to the element, a low temperature is preferable, for example, a temperature lower than 100° C., preferably 40° C. or higher and 90° C. or lower, more preferably 60° C. or higher and 85° C. or lower. The heating time varies depending on the heating temperature, but is, for example, 60 minutes or longer and 120 minutes or shorter.

[0090] In the above embodiment, in step 3), when light is irradiated, acid is generated from the photocationic polymerization initiator. However, because the acid is captured by the tertiary amine, the viscosity does not increase excessively, and a relatively low viscosity can be maintained. Therefore, even in the case of a curable composition containing an inorganic filler, the fluidity and tackiness are unlikely to be impaired when bonding in step 4). Furthermore, in step 5), the acid captured by the tertiary amine is released by heating, and the curable compound cures at a low temperature. As a result, sufficient adhesive strength can be obtained even in the case of a curable composition containing an inorganic filler.

[0091] In the above embodiment, the curable composition is mainly used as a sealant for organic EL elements, but the present invention is not limited thereto and the curable composition can also be used as a sealant or adhesive for various elements such as LED elements (including micro LEDs), liquid crystal elements, semiconductor elements, solar cell elements, etc., or as an interlayer filler for touch panels. The curable composition can also be used as a sealant or adhesive applied to a substrate that does not have optical transparency, such as a printed circuit board used in a smart antenna for an electric vehicle or a substrate having a light-shielding portion under wiring used in a dye-sensitized solar cell.

[0092] The present invention will be further described below with reference to examples and comparative examples, but the technical scope of the present invention is not limited thereto.

[0093] 1. Preparation of materials 1-1. Curable compound (A) Curable compound (A-1): Aromatic trifunctional epoxy compound (VG3101L, manufactured by Printec Co., Ltd., 2-(glycidyloxyphenyl)propylphenyl)-1,1-di(glycidyloxyphenyl)ethane, solid) Curable compound (A-2): Bisphenol F type epoxy resin (YL983U, manufactured by Mitsubishi Chemical Corporation, bifunctional, liquid)

[0094] 1-2. Photocationic polymerization initiator (B) CPI-210S (manufactured by San-Apro Co., Ltd.)

[0095] 1-3. Tertiary amine (C) A compound represented by the following formula (Tinuvin 123, manufactured by BASF Japan Ltd.):

[0096] 1-4. Inorganic filler (D) Inorganic filler (D-1): spherical silica (manufactured by Tokuyama Corporation, Sign Seal SP07M, average particle size 0.7 μm) Inorganic filler (D-2): finely powdered silica (manufactured by Tokuyama Corporation, HM-30S, average particle size 7 nm)

[0097] 1-5. Photosensitizer (E) UVS-1331 (manufactured by Airwater Corporation)

[0098] 1-6. Silane coupling agent (F) KBM403 (manufactured by Shin-Etsu Chemical Co., Ltd.)

[0099] 2. Preparation of Curable Composition Example 1 100 parts by mass of the curable compound (A-1), 200 parts by mass of the curable compound (A-2), 15 parts by mass of the photocationic polymerization initiator (B), 5 parts by mass of the tertiary amine (C), 500 parts by mass of the inorganic filler (D-1), 20 parts by mass of the inorganic filler (D-2), 5 parts by mass of the photosensitizer (E), and 30 parts by mass of the silane coupling agent (F) were mixed in a roll kneader to obtain a curable composition.

[0100] Example 2, Comparative Example 1 Curable compositions were obtained in the same manner as in Example 1, except that the blending amounts of each component were changed as shown in Table 1.

[0101] 3. Evaluation The curable compositions obtained in Examples 1 and 2 and Comparative Example 1 were evaluated for (1) viscosity, (2) tackiness after light irradiation, (3) moisture permeation rate, and (4) adhesive strength by the following methods.

[0102] (1) Viscosity (before and after light irradiation) The viscosity of the obtained curable composition was measured at 25°C using an E-type viscometer (TVE-35L type viscometer, manufactured by Toki Sangyo Co., Ltd., rotor name: 3° × R9.7) in accordance with the cone and plate viscometer method of JIS K5600-2-3 (2014). The rotation speed of the cone and plate during measurement was 2.5 rotations / minute.

[0103] Next, a 10 μm thick coating film of the curable composition was formed on a 0.7 mm thick non-alkali glass plate using a bar coater No. 6. The coating film was left at room temperature (25° C.) for 3 minutes while purging with nitrogen. Thereafter, the coating film was irradiated with ultraviolet light from a metal halide lamp with a wavelength of 365 nm at a UV irradiance of 100 mW / cm. 2The cumulative light intensity is 3000 mJ / cm 2 After irradiation, the coating film was scraped off, and the viscosity after 60 seconds was measured in the same manner as above.

[0104] (2) Tack after light irradiation Using the obtained curable composition, a coating film having a thickness of 10 μm was formed on a 0.7 mm thick non-alkali glass plate using a bar coater No. 6. The coating film was left at room temperature (25° C.) for 3 minutes while purging with nitrogen. Thereafter, the coating film was irradiated with ultraviolet light (a metal halide lamp with a wavelength of 365 nm, UV irradiance 100 mW / cm). 2 The cumulative light intensity is 3000 mJ / cm 2 ) was irradiated. Then, the coating film was touched with a hand wearing a protective device to check for tackiness. If tackiness was present, it was rated as "present," and if no tackiness was present, it was rated as "absent."

[0105] (3) Moisture Permeability The obtained curable composition was applied to a release paper with an applicator to a thickness of 100 μm. The applied curable composition was then placed in a nitrogen-purging container and purged with nitrogen for 5 minutes. After that, the moisture permeability was measured at 3000 mJ / cm. 2 The coating was then irradiated with light (calibrated with a 365 nm wavelength sensor) and further heated at 120° C. for 1 hour to cure, producing a film made of a cured product.

[0106] Two sheets of cured film were placed on an aluminum cup containing calcium chloride (anhydrous) as a moisture absorbent, and an aluminum ring was placed on top and screwed in place, after which the initial weight of the entire aluminum cup was measured. The aluminum cup was then placed in a thermostatic chamber set to 60°C and 90% Rh, and after 24 hours had passed, the aluminum cup was removed and its weight was measured. The obtained weight value was substituted into the following formula to calculate the moisture permeability. Moisture permeability (g / m 2 24h) = (weight after test - weight before test) x film thickness / (film area x 100) Moisture permeability 50g / m 2 If it is less than 50 g / m, it is judged to be good. 2 If it exceeded this, it was judged to be defective.

[0107] (4) Adhesion Strength The obtained curable composition was applied in a circular pattern using a screen on a non-alkali glass sheet measuring 25 mm x 45 mm x 0.7 mm. The seal pattern was a circle with a diameter of 1 mm. Next, the coating of the curable composition was irradiated with light having a wavelength of 365 nm at an irradiation intensity of 100 mW / cm. 2 After irradiating one of the alkali-free glass sheets with a 0.7 mm thickness for 30 seconds, a pair of alkali-free glass sheets was bonded together and heated in an oven at 80°C for 60 minutes to obtain a laminate sample. The obtained sample was then aged for 24 hours in a thermostatic chamber at 23°C, and then pulled in a tensile testing machine (Intesco Model 210 tensile testing machine) in a direction parallel to the surface at a rate of 2 mm / min, and the stress at this time was measured.

[0108] The evaluation results of the curable compositions of Examples 1 and 2 and Comparative Example 1 are shown in Table 1.

[0109]

[0110] As shown in Table 1, the curable composition of Comparative Example 1, which did not contain a tertiary amine, showed no tack after light irradiation and the adhesive strength of the cured product was low.

[0111] In contrast, the curable compositions of Examples 1 and 2, which contain a predetermined amount or more of tertiary amine, are found to retain tackiness after light irradiation, and the adhesive strength of the cured product is also found to be high.

[0112] From these findings, it can be seen that even when an inorganic filler is contained, by using a photocationic polymerization initiator in combination with a predetermined amount or more of a tertiary amine, the viscosity after light irradiation can be kept low and the low-temperature curing properties are also excellent.

[0113] This application claims priority from Japanese Patent Application No. 2023-54118, filed March 29, 2023, the entire contents of which are incorporated herein by reference.

[0114] According to the present invention, it is possible to provide a curable composition that has both low-temperature curing properties and viscosity stability after light irradiation, and that can give a cured product that has low moisture permeability and high adhesive strength.

Claims

1. A curable composition comprising a curable compound, a photocationic polymerization initiator, a tertiary amine, and an inorganic filler, wherein the content of the tertiary amine is 20 parts by mass or more per 100 parts by mass of the photocationic polymerization initiator.

2. The curable composition according to claim 1, wherein the content of the tertiary amine is 0.5 parts by mass or more and 20 parts by mass or less per 100 parts by mass of the curable compound.

3. The curable composition according to claim 1, wherein the content of the inorganic filler is 20 parts by mass or more and 400 parts by mass or less per 100 parts by mass of the curable compound.

4. The curable composition according to claim 1, wherein the curable compound comprises an aromatic epoxy compound.

5. The curable composition according to claim 1, wherein the tertiary amine is a difunctional tertiary amine.

6. The curable composition according to claim 1, wherein the tertiary amine has an N--O bond.

7. The curable composition according to claim 1, wherein the tertiary amine has a hindered structure.

8. 365 nm wavelength light with UV irradiance of 100 mW / cm 2 With an integrated light intensity of 3000 mJ / cm 2 After irradiation, the viscosity at 25°C 60 seconds later was 1.0 x 10 4 The curable composition according to claim 1 , having a viscosity of not more than Pa·s.

9. A sealant comprising the curable composition according to any one of claims 1 to 8.

10. A frame sealant comprising the curable composition according to any one of claims 1 to 8.

11. A display panel comprising: an element substrate on which elements are arranged; an opposing substrate arranged opposite the element substrate with the elements interposed therebetween; and a sealing portion arranged between the element substrate and the opposing substrate for sealing the elements, the sealing portion including a cured product of the sealant according to claim 9.

12. A method for manufacturing a display panel, comprising: a step of applying a first sealant in a frame shape along the periphery of a display area on one surface of either an element substrate or an opposing substrate; a step of filling a second sealant into the area surrounded by the first sealant to form a sealant layer; a step of irradiating the sealant layer with light; a step of bonding one substrate to the other substrate via the sealant layer irradiated with light; and a step of heating and hardening the sealant layer, wherein at least one of the first sealant and the second sealant is the sealant described in claim 9.

13. The method for manufacturing a display panel according to claim 12, wherein the first sealant is the sealant according to claim 9.

Citation Information

Patent Citations

  • Irradiation-cured anti-fouling coiled material coating and preparation method thereof

    CN110885619A

  • Cellulose acylate film, optical film using the film, liquid crystal display device and silver halide photosensitive material

    JP2004099775A

  • Ink, image-forming method, print and recording device

    JP2004238456A

  • Stain resistance-imparting agent, cured product and article

    JP2006160802A

  • Active energy beam-curable composition and ink for inkjet

    JP2009275080A