Polarizer protection film, polarizing plate, and liquid crystal panel

The polarizer protective film with an acrylic resin composition and specific properties addresses the issue of uneven display and yellowness in IPS type liquid crystal panels by ensuring uniform in-plane retardation and reduced yellowness, improving the color rendering and stability of the panels.

WO2024204295A1PCT designated stage expired Publication Date: 2024-10-03KANEKA CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012147
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Polarizer protective films containing acrylic resin cause uneven display and a yellowish appearance when viewed from an oblique direction in IPS type liquid crystal panels, due to variations in in-plane retardation and color tone issues.

Method used

A polarizer protective film with an acrylic resin composition having a ring structure in the main chain, specific retardation values, and birefringence properties, which is biaxially stretched and optimized for uniform in-plane retardation and reduced yellowness, is developed. The film has a thickness direction retardation of -15.0 nm or more and less than 0.0 nm at 590 nm, with a glass transition temperature of 120°C or higher, and includes structural units derived from methyl methacrylate and styrene, ensuring improved mechanical properties and color rendering.

Benefits of technology

The solution achieves uniform in-plane retardation and reduces yellowness when viewed from an oblique direction, enhancing the color rendering properties and stability of the liquid crystal panel, particularly in high temperature and humidity environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

Provided is a polarizer protection film including an acrylic resin composition and having a retardation Rth in the thickness direction at a wavelength of 590 nm of -15.0 nm to less than 0.0 nm, wherein the acrylic resin composition includes an acrylic resin having a ring structure in the main chain thereof, has a glass transition temperature of 120°C or higher, and has a birefringence development Δnxy of -1.0 × 10-3 to -0.1 × 10-3.
Need to check novelty before this filing date? Find Prior Art

Description

Polarizer protective film, polarizing plate and liquid crystal panel

[0001] The present invention relates to a polarizer protective film, a polarizing plate, and a liquid crystal panel.

[0002] Acrylic resins have excellent transparency, color tone, appearance, heat resistance, and processability, and are therefore used in, for example, polarizer protective films (see, for example, Patent Document 1). Here, the polarizer protective films are attached to both sides of a polarizer to form polarizing plates, which are then placed on both sides of a liquid crystal cell to be used in liquid crystal panels.

[0003] On the other hand, IPS type liquid crystal panels are preferably used for applications such as liquid crystal televisions because of their wide viewing angle and excellent color reproducibility.

[0004] JP 2017-25333 A

[0005] However, when a polarizer protective film containing an acrylic resin is applied to an IPS-type liquid crystal panel, the liquid crystal panel may have a slight yellowish tinge when displayed in black and viewed from an oblique direction. On the other hand, when such a color tone problem is optically compensated for by the retardation of the polarizer protective film, variations in the in-plane retardation of the polarizer protective film may cause unevenness in the display of the liquid crystal panel.

[0006] An object of the present invention is to provide a polarizer protective film that can achieve both uniformity of in-plane retardation and reduction in yellowness when viewed from an oblique direction of a liquid crystal panel.

[0007] [1] An optical fiber comprising an acrylic resin composition, having a thickness direction retardation Rth of −15.0 nm or more and less than 0.0 nm at a wavelength of 590 nm, the acrylic resin composition comprising an acrylic resin having a ring structure in its main chain, a glass transition temperature of 120° C. or more, and a birefringence development index Δnxy of −1.0×10 -3 Above -1.0 x 10 -4 The polarizer protective film is as follows.

[0008] [2] The polarizer protective film described in (1), wherein the acrylic resin having a ring structure in its main chain has a structural unit including, in its main chain, one or more ring structures selected from the group consisting of a glutarimide ring, a lactone ring, a maleic anhydride ring, a maleimide ring, and a glutaric anhydride ring.

[0009] [3] The polarizer protective film according to [2], wherein the acrylic resin having a ring structure in its main chain has a structural unit represented by the following formula (1):

[0010] (In the formula, R 1 and R 2 are each independently a hydrogen atom or an alkyl group having 1 to 8 carbon atoms, and R 3 is a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, or a cycloalkyl group having 3 to 12 carbon atoms.

[0011] [4] The polarizer protective film according to any one of [1] to [3], wherein the acrylic resin composition has a content of structural units derived from aromatic vinyl of 0% by weight or more and 8% by weight or less.

[0012] [5] The polarizer protective film according to [4], wherein the acrylic resin composition has a content of structural units derived from styrene of 0% by weight or more and 8% by weight or less.

[0013] [6] The polarizer protective film according to any one of [1] to [5], wherein the acrylic resin composition further contains polymethyl methacrylate or a methyl methacrylate-styrene copolymer.

[0014] [7] The polarizer protective film according to any one of [1] to [6], wherein the acrylic resin composition has a 1% weight loss temperature of 300°C or higher.

[0015] [8] The polarizer protective film according to any one of [1] to [7], which does not contain an ultraviolet absorber.

[0016] [9] The polarizer protective film according to any one of [1] to [8], which is a biaxially stretched film.

[0017]

[10] The polarizer protective film according to any one of [1] to [9], which has a yellowness index of 0.01 or more and 5.00 or less.

[0018]

[11] The polarizer protective film according to any one of [1] to

[10] , which has an absorbance at a wavelength of 380 nm of 0.01 or more and 1.00 or less.

[0019]

[12] The polarizer protective film according to any one of [1] to

[11] , wherein the absolute value of the Nz coefficient is 0.1 or more and 30.0 or less, the ratio Rth(447) / Rth(548) of the thickness direction retardation Rth(447) at a wavelength of 447 nm to the thickness direction retardation Rth(548) at a wavelength of 548 nm is 0.50 or more and 1.10 or less, and the ratio Rth(628) / Rth(548) of the thickness direction retardation Rth(628) at a wavelength of 628 nm to the thickness direction retardation Rth(548) at a wavelength of 548 nm is 0.50 or more and 2.00 or less.

[0020]

[13] A polarizing plate comprising the polarizer protective film according to any one of [1] to

[12] .

[0021]

[14] A liquid crystal panel comprising the polarizing plate according to

[13] .

[0022] According to the present invention, it is possible to provide a polarizer protective film that can achieve both uniformity of in-plane retardation and reduction in yellowness when viewed from an oblique direction of a liquid crystal panel.

[0023] Hereinafter, an embodiment of the present invention will be described.

[0024] (Polarizer Protective Film) The polarizer protective film of the present embodiment contains an acrylic resin composition.

[0025] The thickness direction retardation Rth at a wavelength of 590 nm of the polarizer protective film of this embodiment is −15.0 nm or more and less than 0.0 nm, preferably −13.0 nm or more and less than −2.5 nm, more preferably −10.0 nm or more and less than −2.5 nm, more preferably −10.0 nm or more and less than −5.0 nm, and particularly preferably −10.0 nm or more and less than −7.0 nm. When Rth is −15.0 nm or more and less than 0.0 nm, the yellowness index when viewed from an oblique direction of the liquid crystal panel is reduced. In this case, the polarizer protective film of this embodiment preferably has a yellowness index of 50 or less when viewed from an oblique direction of the liquid crystal panel.

[0026] The average in-plane retardation Re of the polarizer protective film of this embodiment is preferably greater than 0.0 nm and equal to or less than 0.7 nm, more preferably equal to or less than 0.6 nm. When the average Re is equal to or less than 0.7 nm, the uniformity of the in-plane retardation Re is improved. In this case, the polarizer protective film of this embodiment preferably has a standard deviation of the in-plane retardation Re of less than 0.2.

[0027] Re and Rth are calculated by the formulas: Re = (nx - ny) x d, Rth = [(nx + ny) / 2 - nz] x d. Here, nx, ny, and nz are the refractive indices in the X-axis direction, Y-axis direction, and Z-axis direction, respectively, where the MD direction is the X-axis, the TD direction is the Y-axis, and the thickness direction of the film is the Z-axis. Also, d is the thickness of the film.

[0028] The yellowness index of the polarizer protective film of this embodiment is preferably 0.01 or more and 5.00 or less, and more preferably 0.1 or more and 2.0 or less. When the yellowness index of the polarizer protective film of this embodiment is 5.00 or less, the polarizer protective film of this embodiment is less colored and has less effect on the color rendering properties of the display.

[0029] The absorbance of the polarizer protective film of this embodiment at a wavelength of 380 nm is preferably 0.01 or more and 1.00 or less, and more preferably 0.10 or more and 0.80 or less. When the absorbance of the polarizer protective film of this embodiment at a wavelength of 380 nm is 1.00 or less, the polarizer protective film of this embodiment is substantially free of an ultraviolet absorber.

[0030] The absolute value of the Nz coefficient of the polarizer protective film of this embodiment is preferably 0.1 or more and 30.0 or less. When the absolute value of the Nz coefficient of the polarizer protective film of this embodiment is 0.1 or more and 30.0 or less, the yellowness when viewed from an oblique direction of the liquid crystal panel is reduced.

[0031] The ratio Rth(447) / Rth(548), which is the thickness direction retardation Rth(447) at a wavelength of 447 nm to the thickness direction retardation Rth(548) at a wavelength of 548 nm, of the polarizer protective film of this embodiment is preferably 0.50 or more and 1.10 or less, more preferably 0.80 or more and 1.08 or less. When Rth(447) / Rth(548) of the polarizer protective film of this embodiment is 0.50 or more and 1.10 or less, the yellowness when viewed from an oblique direction of the liquid crystal panel is reduced.

[0032] The ratio Rth(628) / Rth(548), which is the thickness direction retardation Rth(628) at a wavelength of 628 nm to the thickness direction retardation Rth(548) at a wavelength of 548 nm, of the polarizer protective film of this embodiment is preferably 0.50 or more and 2.00 or less, and more preferably 0.7 or more and 1.5 or less. When Rth(628) / Rth(548) of the polarizer protective film of this embodiment is 0.50 or more and 2.00 or less, the yellowness when viewed from an oblique direction of the liquid crystal panel is reduced.

[0033] The photoelastic coefficient of the polarizer protective film of this embodiment is −10×10 -12 Pa -1 10 x 10 or more -12 Pa -1 It is preferable that the value is equal to or less than -5.5 × 10 -12 Pa -1 5.5 x 10 -12 Pa -1More preferably, it is −4.5×10 or less. -12 Pa -1 4.5 x 10 -12 Pa -1 It is more preferable that the photoelastic coefficient of the polarizer protective film of the present embodiment is −10×10 or less. -12 Pa -1 10 x 10 or more -12 Pa -1 When the thickness is not more than this, the polarizer protective film of the present embodiment is less likely to suffer from color unevenness, and this tendency becomes particularly pronounced under high-temperature and high-humidity environments.

[0034] (Acrylic Resin Composition) The acrylic resin composition contains an acrylic resin having a ring structure in the main chain. The glass transition temperature of the acrylic resin composition is 120°C or higher, preferably greater than 120°C, more preferably 121°C or higher, and even more preferably 122°C or higher. If the glass transition temperature of the acrylic resin composition is lower than 120°C, orientation relaxation may proceed in a high-temperature, high-humidity environment, resulting in a decrease in retardation stability. The glass transition temperature of the acrylic resin composition is, for example, 160°C or lower.

[0035] In this specification and claims, acrylic resin refers to a polymer of a monomer having an acryloyl group and / or a monomer having a methacryloyl group. In this case, the acrylic resin may be either a homopolymer or a copolymer. When the acrylic resin is a copolymer, it may be a copolymer of a monomer not having an acryloyl group or a methacryloyl group.

[0036] The birefringence development Δnxy of the acrylic resin composition is −1.0×10 -3 Above -0.1 x 10 -3 is less than or equal to -0.8 × 10 -3 Above -0.25 x 10 -3 It is preferable that the value is less than or equal to -0.8 × 10 -3 Above -0.20 x 10 -3 More preferably, it is −0.8×10 or less. -3 Above -0.12 x 10 -3 It is more preferable that Δnxy is −1.0×10 or less.-3 When the film is biaxially stretched, the desired thickness direction retardation is easily exhibited, and the film is −0.1×10 -3 If it is less than this, the in-plane retardation tends to be uniform when biaxially stretched.

[0037] In this specification and claims, the birefringence development property Δnxy of an acrylic resin composition means birefringence developed when a film of the acrylic resin composition in an unstretched state is uniaxially stretched at its free end to a stretching ratio of 2 in the machine direction (longitudinal direction) at a temperature 5°C higher than the glass transition temperature of the acrylic resin composition.

[0038] Δnxy is calculated by the formula Δnxy=nx-ny=Re / d, where nx and ny are the refractive indices in the X-axis and Y-axis directions, respectively, when the MD direction is the X-axis, the TD direction is the Y-axis, and the thickness direction of the film is the Z-axis. Re is the in-plane retardation of the film, and d is the thickness of the film.

[0039] The acrylic resin composition may further contain, for example, polymethyl methacrylate or a methyl methacrylate-styrene copolymer. It is preferable that the acrylic resin contained in the acrylic resin composition does not have a structural unit derived from an aromatic vinyl.

[0040] The content of structural units derived from aromatic vinyl (e.g., styrene) in the acrylic resin composition is preferably 0 wt% or more and 8 wt% or less, more preferably 0.5 wt% or more and 5 wt% or less, even more preferably 0.5 wt% or more and 3 wt% or less, even more preferably 0.5 wt% or more and 2.5 wt% or less, and particularly preferably 1.0 wt% or more and 2.5 wt% or less. When the content of structural units derived from aromatic vinyl (e.g., styrene) in the acrylic resin composition is 8 wt% or less, the uniformity of the in-plane retardation of the polarizer protective film of this embodiment is improved.

[0041] The acrylic resin composition may further contain additives within a range that does not impair the object of the present invention. The additives are not particularly limited, but examples thereof include antioxidants, heat stabilizers, light stabilizers, ultraviolet absorbers, specific wavelength absorbers or specific wavelength absorbing dyes for cutting blue light, light resistance stabilizers such as radical scavengers, retardation adjusters, catalysts, plasticizers, lubricants, antistatic agents, colorants, shrinkage inhibitors, antibacterial and deodorizing agents, fluorescent brighteners, and compatibilizers, and two or more of these may be used in combination.

[0042] The 1% weight loss temperature of the acrylic resin composition is preferably 300°C or higher, more preferably 302°C or higher, and even more preferably 305°C or higher. When the 1% weight loss temperature of the acrylic resin composition is 300°C or higher, contamination of the cooling roll during production of the raw film is suppressed, and the film formability of the raw film is improved. The 1% weight loss temperature of the raw film is, for example, 380°C or lower.

[0043] The weight-average molecular weight of the acrylic resin composition is preferably from 50,000 to 200,000, and more preferably from 90,000 to 150,000. When the weight-average molecular weight of the acrylic resin composition is 50,000 or more, the mechanical properties of a molded product of the acrylic resin composition tend to be improved, and when it is 200,000 or less, the moldability of the acrylic resin composition tends to be improved.

[0044] The ratio of the weight average molecular weight to the number average molecular weight of the acrylic resin composition (polydispersity) is preferably 1.5 or more and 2.5 or less, and more preferably 1.5 or more and 2.2 or less. When the polydispersity of the acrylic resin composition is 1.5 or more, the flowability of the acrylic resin composition tends to be improved and it tends to be easy to mold, and when it is 2.5 or less, the mechanical properties such as impact resistance, toughness, and flex resistance of an article molded from the acrylic resin composition tend to be improved.

[0045] The number-average molecular weight and weight-average molecular weight of the acrylic resin composition are values ​​measured by gel permeation chromatography (GPC) in terms of standard polystyrene. The number-average molecular weight and weight-average molecular weight of the acrylic resin composition can be controlled by the types and amounts of polymerization initiators and chain transfer agents used in synthesizing the acrylic resin.

[0046] The polarizer protective film of this embodiment can be attached to a polarizer to form a polarizing plate. The polarizer is not particularly limited, and a known polarizer can be used. The polarizing plate can also be combined with a liquid crystal cell to form a liquid crystal panel. In this case, it is preferable to use an IPS-type liquid crystal cell with a wide viewing angle. When the polarizer protective film of this embodiment is disposed on the side facing the liquid crystal cell, it may not contain an ultraviolet absorber, or may not substantially contain an ultraviolet absorber.

[0047] (Acrylic Resin Having a Ring Structure in the Main Chain) The acrylic resin having a ring structure in the main chain (hereinafter referred to as "acrylic resin") preferably has a structural unit containing, in the main chain, one or more ring structures selected from the group consisting of a glutarimide ring, a lactone ring, a maleic anhydride ring, a maleimide ring, and a glutaric anhydride ring.

[0048] The structural unit containing a glutarimide ring in the main chain is represented by, for example, the following formula (1).

[0049] (In the formula, R 1 and R 2 are each independently a hydrogen atom or an alkyl group having 1 to 8 carbon atoms, and R 3 is a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, or a cycloalkyl group having 3 to 12 carbon atoms.

[0050] The acrylic resin having the structural unit represented by formula (1) can be produced by a known method. An example of a method for producing the acrylic resin having the structural unit represented by formula (1) will be described below.

[0051] First, a twin-screw extruder equipped with a die at the outlet is used to melt the methyl methacrylate resin, which is then imidized, and a strand is extruded from the die. Next, the strand is cooled using a water bath and then pelletized using a pelletizer to obtain an imidized methyl methacrylate resin. Next, a twin-screw extruder equipped with a die at the outlet is used to melt the imidized methyl methacrylate resin, which is then esterified, and a strand is extruded from the die. Next, the strand is cooled using a water bath and then pelletized using a pelletizer to obtain an acrylic resin having a structural unit represented by formula (1).

[0052] Examples of the imidizing agent include ammonia and primary amines represented by the following formula (2): Among these, monomethylamine is preferred.

[0053] R 3 NH 2 (2) (wherein, R 3 is synonymous with formula (1).

[0054] Examples of the esterifying agent include dimethyl carbonate, 2,2-dimethoxypropane, dimethyl sulfoxide, triethyl orthoformate, trimethyl orthoacetate, trimethyl orthoformate, diphenyl carbonate, dimethyl sulfate, methyl toluene sulfonate, methyl trifluoromethyl sulfonate, methyl acetate, methanol, ethanol, methyl isocyanate, p-chlorophenyl isocyanate, dimethylcarbodiimide, dimethyl-t-butylsilyl chloride, isopropenyl acetate, dimethyl urea, tetramethylammonium hydroxide, dimethyldiethoxysilane, tetra-n-butoxysilane, dimethyl(trimethylsilane) phosphite, trimethyl phosphite, trimethyl phosphate, tricresyl phosphate, diazomethane, ethylene oxide, propylene oxide, cyclohexene oxide, 2-ethylhexyl glycidyl ether, phenyl glycidyl ether, and benzyl glycidyl ether. Of these, dimethyl carbonate is preferred.

[0055] The content of the structural unit containing a ring structure in the main chain in the acrylic resin is preferably 1% by weight or more and 80% by weight or less, and the glass transition temperature of the acrylic resin is preferably 120°C or more and 160°C or less.

[0056] The acrylic resin may further contain a structural unit derived from a (meth)acrylic acid ester.

[0057] Examples of (meth)acrylic acid esters include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, and isobutyl (meth)acrylate; aryl (meth)acrylates such as phenyl (meth)acrylate; aralkyl (meth)acrylates such as benzyl (meth)acrylate; and cycloalkyl (meth)acrylates such as cyclohexyl (meth)acrylate, and two or more of these may be used in combination. Among these, alkyl methacrylates are preferred, and methyl methacrylate is particularly preferred.

[0058] The content of structural units derived from alkyl methacrylate in the acrylic resin is preferably 50% by weight or more, more preferably 75% by weight or more, and particularly preferably 90% by weight or more.

[0059] The content of structural units derived from acrylic acid ester in the acrylic resin is preferably less than 1% by weight, more preferably less than 0.5% by weight, and particularly preferably less than 0.3% by weight.

[0060] The acrylic resin may further contain structural units derived from other monomers, including, but not limited to, aromatic monomers such as styrene and methylstyrene, and nitrile monomers such as acrylonitrile and methacrylonitrile.

[0061] (Method for Producing Polarizer Protective Film) The polarizer protective film of the present embodiment can be produced by a known method. An example of the method for producing the polarizer protective film of the present embodiment will be described below.

[0062] First, an acrylic resin is kneaded, if necessary, together with a methyl methacrylate-styrene copolymer using an extruder equipped with a die at the outlet, and a strand is extruded from the die. Next, the strand is cooled using a water tank and then pelletized using a pelletizer to obtain an acrylic resin composition. Next, the acrylic resin composition is melted using an extruder equipped with a T-die at the outlet, and a sheet is extruded from the T-die and cooled with a cooling roll to obtain a raw film. Next, the raw film is biaxially stretched to obtain the polarizer protective film of this embodiment. In this case, the biaxial stretching may be simultaneous biaxial stretching or sequential biaxial stretching.

[0063] The temperature when biaxially stretching the raw film is preferably (Tg + 5) ° C. or higher (Tg + 20) ° C. or lower, more preferably (Tg + 6) ° C. or higher (Tg + 18) ° C. or lower, and even more preferably (Tg + 7) ° C. or higher (Tg + 15) ° C. or lower, where Tg is the glass transition temperature of the acrylic resin composition. The areal magnification when biaxially stretching the raw film is not particularly limited, but is, for example, 2 times or higher and 10 times or lower. The stretching speed when biaxially stretching the raw film is not particularly limited, but is, for example, 1.1 times / min. or higher and 100 times / min. When sequentially biaxially stretching the raw film, the first-stage stretching speed and the second-stage stretching speed may be the same or different. In sequential biaxial stretching, the first-stage stretching is usually stretching in the longitudinal direction (MD direction), and the second-stage stretching is stretching in the width direction (TD direction).

[0064] Although the embodiments of the present invention have been described above, the present invention is not limited to the above-described embodiments, and the above-described embodiments may be modified as appropriate within the scope of the spirit of the present invention.

[0065] Examples of the present invention will be described below, but the present invention is not limited to these examples.

[0066] (Content of structural units containing glutarimide rings in the main chain) Using a nuclear magnetic resonance apparatus Avance III (manufactured by BRUKER) with a proton resonance frequency of 400 MHz, 1The H-NMR spectrum was measured. The molar ratio of the structural unit derived from methyl methacrylate to the structural unit containing a glutarimide ring in the main chain was converted into weight, and the content of the structural unit containing a glutarimide ring in the main chain was calculated. At this time, the O—CH 3 The peak area A due to protons and the N-CH of glutarimide at around 3.0 to 3.3 ppm 3 The molar ratio was calculated from the peak area B derived from protons.

[0067] (Glass Transition Temperature) Using a high-sensitivity differential scanning calorimeter DSC7000X (manufactured by Hitachi High-Tech Science), 10 mg of an acrylic resin or an acrylic resin composition was heated at a heating rate of 10°C / min in a nitrogen atmosphere, and the glass transition temperature was determined by the midpoint method.

[0068] (1% Weight Loss Temperature) Using a thermogravimetric and differential scanning calorimeter STA7200 (manufactured by Hitachi High-Tech Science), 10 mg of the acrylic resin composition was heated from room temperature at a heating rate of 10°C / min in a nitrogen atmosphere to determine the 1% weight loss temperature.

[0069] (Birefringence development Δnxy) After cutting out a 30 × 100 mm area from the raw film, the raw film was subjected to free-end uniaxial stretching at a temperature 5 ° C. higher than the glass transition temperature of the raw film so that the stretching ratio in the machine direction (longitudinal direction) was 2 times, thereby obtaining a uniaxially stretched film. Next, using a retardation measuring device KOBRA-WR (manufactured by Oji Scientific Instruments), the in-plane retardation of the central part of the uniaxially stretched film was measured, and then divided by the thickness of the uniaxially stretched film to obtain birefringence development Δnxy.

[0070] (Thickness Direction Retardation Rth) The thickness direction retardation Rth of the polarizer protective film was measured at a wavelength of 590 nm using a retardation measuring device KOBRA-WR (manufactured by Oji Scientific Instruments).

[0071] (Average value and standard deviation of in-plane retardation Re) After cutting out a central 150 × 150 mm range from the polarizer protective film, the average value and standard deviation of the in-plane retardation Re were measured using a two-dimensional birefringence evaluation system WPA-200 (manufactured by Photonic Lattice Co., Ltd.). At this time, after drawing three lines in each of the MD and TD directions, the average value and standard deviation of the in-plane retardation Re were determined using a line analysis function.

[0072] (Yellowness Index) After cutting the polarizer protective film into a 3 cm square, the yellowness index (YI) was measured using a color meter SC-P (manufactured by Suga Test Instruments) in accordance with JIS K7373:2006.

[0073] (Absorbance at a Wavelength of 380 nm) The absorbance of the polarizer protective film at a wavelength of 380 nm was measured using an ultraviolet-visible-near-infrared spectrophotometer UV-560 (manufactured by JASCO Corporation).

[0074] (Photoelastic Coefficient) The photoelastic coefficient of the polarizer protective film was measured using a KOBRA retardation measurement device (manufactured by Oji Scientific Instruments). Specifically, the polarizer protective film was cut into a size of 15 mm x 60 mm, and the change in retardation was measured when a tensile load was applied from 0 g to 1100 g in increments of 100 g. The stress calculated from the tensile load value was plotted on the X axis, and the birefringence calculated from the measured retardation and film thickness was plotted on the Y axis. The slope of the straight line in the plotted graph was calculated to be the photoelastic coefficient.

[0075] (Yellowness Index When Viewed Obliquely from the Liquid Crystal Panel) A liquid crystal panel simulation was performed using a liquid crystal simulator, LCD Master (manufactured by Shintech). A polarizing plate disposed on the light source side, an IPS-type liquid crystal cell having an in-plane retardation Re of 295 nm, and a polarizing plate disposed on the viewing side were arranged in this order. Measurement results of the thickness direction retardation Rth were input as the optical properties of the polarizer protective film on the side of the polarizing plate disposed on the light source side and the viewing side facing the liquid crystal cell. Next, the XYZ colorimetric values ​​when viewed from a polar angle of 70° and an azimuthal angle of 40° with the liquid crystal cell set in a dark state were determined by simulation, and the yellowness index (YI) was calculated from the following formula in accordance with JIS K7373:2006. YI=100(1.2985X-1.1335Z) / Y

[0076] (Rth(447) / Rth(548), Rth(628) / Rth(548) and Nz Coefficient) Using a retardation measurement device KOBRA-WR (manufactured by Oji Scientific Instruments), the retardation of the polarizer protective film at wavelengths λ (λ = 446.7 nm, 547.9 nm, 628.2 nm) was measured. Specifically, the in-plane retardation Re(λ) at each wavelength and the retardation R40(λ) measured at a 40° tilt with the absorption axis as the tilt axis were measured, and then the three-dimensional refractive index calculation software N-Calc (manufactured by Oji Scientific Instruments) was used to calculate the three-dimensional refractive indexes nx(λ), ny(λ), and nz(λ) at each wavelength. Next, using the three-dimensional refractive indices nx (λ), ny (λ), and nz (λ), the thickness direction retardation Rth (λ) at each wavelength was calculated by the formula Rth (λ) = [{nx (λ) + ny (λ)} / 2 - nz (λ)] × d, and the wavelength dispersion characteristics Rth (447) / Rth (548), Rth (628) / Rth (548) were obtained. In addition, using the in-plane retardation Re (548) and thickness direction retardation Rth (548) at a wavelength of 548 nm, the Nz coefficient was calculated by the formula Nz coefficient = [Rth (548) / Re (548)] + 0.5.

[0077] (Weight-average molecular weight, number-average molecular weight, and polydispersity index) The weight-average molecular weight (Mw), number-average molecular weight (Mn), and polydispersity index (Mw / Mn) of the acrylic resin composition were calculated using gel permeation chromatography (GPC). The analysis was carried out under the following conditions using a sample solution prepared by dissolving 20 mg of the acrylic resin composition in 10 mL of tetrahydrofuran. Measuring instrument: HLC-8420GPC (manufactured by Tosoh Corporation) Detector: RI detector Eluent: tetrahydrofuran Guard column: TSKgel guard column Super H-L (manufactured by Tosoh Corporation) Analytical column: TSKgel Super H5000, Super H4000, Super H3000, Super H2000 (manufactured by Tosoh Corporation) (in series) Eluent flow rate: 0.6 mL / min Measurement temperature: 40°C Standard material: standard polystyrene (manufactured by Tosoh Corporation)

[0078] (Production of Acrylic Resin 1) The temperature of each temperature-controlled zone of a 40 mm diameter co-rotating intermeshing twin-screw extruder (L / D = 90) equipped with a die at the outlet was set to 250 to 280 ° C., the screw rotation speed was 85 rpm, and methyl methacrylate resin Parapet HM (manufactured by Kuraray) was melted and filled using a kneading block. Next, 1.8 wt% of monomethylamine (manufactured by Mitsubishi Gas Chemical Company) was added to the methyl methacrylate resin through the nozzle to imidize the methyl methacrylate resin. Next, the strand extruded from the die was cooled using a water bath, and then the strand was pelletized using a pelletizer to obtain Resin (I).

[0079] The temperature setting for each temperature control zone of a 40 mm diameter co-rotating intermeshing twin-screw extruder (L / D = 90) equipped with a die at the outlet was set to 240-260°C, and the screw rotation speed was set to 85 rpm. Resin (I) was melted and filled using a kneading block. Next, 0.56 wt% of dimethyl carbonate was added to resin (I) through the nozzle to esterify the carboxyl groups in resin (I). At this time, by-products and excess dimethyl carbonate were removed after the reaction. The strands extruded from the die were then cooled in a water bath and pelletized using a pelletizer to obtain acrylic resin 1. Acrylic resin 1 had a glass transition temperature of 123°C and a content of structural units containing glutarimide rings in the main chain of 6 wt%.

[0080] (Production of Acrylic Resin 2) Acrylic Resin 2 was obtained in the same manner as Acrylic Resin 1, except that the amount of monomethylamine added was changed to 4.3% by weight relative to the methyl methacrylate resin. Acrylic Resin 2 had a glass transition temperature of 125°C and a content of structural units containing glutarimide rings in the main chain of 15% by weight.

[0081] (Production of Acrylic Resin 3) Acrylic Resin 3 was obtained in the same manner as Acrylic Resin 1, except that methyl methacrylate-styrene copolymer TX-100 (manufactured by Denka) containing 40% by weight of structural units derived from styrene was used instead of methyl methacrylate resin, and the amount of monomethylamine added was 8.2% by weight relative to the methyl methacrylate-styrene copolymer. Acrylic Resin 5 had a glass transition temperature of 125°C and a content of structural units containing glutarimide rings in the main chain of 45% by weight.

[0082] Table 1 shows the properties of the acrylic resin.

[0083]

[0084] Example 1 Using a 15 mm diameter, co-rotating, intermeshing twin-screw extruder (L / D = 45) equipped with a die at the outlet, 95 wt % of acrylic resin 1 and 5 wt % of methyl methacrylate-styrene copolymer KT-89 (manufactured by Denka) containing 11 wt % of structural units derived from styrene were kneaded. Next, a water bath was used to cool the strand extruded from the die at the outlet of the extruder, and the strand was pelletized using a pelletizer to obtain an acrylic resin composition. The acrylic resin composition had a glass transition temperature of 123°C, a 1% weight loss temperature of 308°C, an Mw of 81,000, and an Mw / Mn of 1.62.

[0085] The acrylic resin composition was dried at 100°C for 5 hours, and then melted using a 15mm diameter, co-rotating, intermeshing twin-screw extruder (L / D = 45) equipped with a T-die at the outlet. The sheet extruded from the T-die was then cooled using a cooling roll to obtain a raw film having a width of 160mm and a thickness of 160µm.

[0086] Using a film biaxial stretching apparatus IMC-1905 (manufactured by Imoto Machinery Works, Ltd.), the raw film was simultaneously biaxially stretched at a temperature 15°C higher than the glass transition temperature of the acrylic resin composition so that the stretching ratio in the longitudinal direction and the transverse direction became 2 times, thereby obtaining a polarizer protective film of 280 mm x 280 mm.

[0087] Example 2 A polarizer protective film was obtained in the same manner as in Example 1, except that the mixing ratios of acrylic resin 1 and KT-89 (manufactured by Denka) were changed to 90% by weight and 10% by weight, respectively. The acrylic resin composition had a glass transition temperature of 123°C, a 1% weight loss temperature of 308°C, an Mw of 81,000, and an Mw / Mn of 1.62.

[0088] Example 3 A polarizer protective film was obtained in the same manner as in Example 2, except that the raw film was simultaneously biaxially stretched at a temperature 7° C. higher than the glass transition temperature of the acrylic resin composition.

[0089] Example 4 A polarizer protective film was obtained in the same manner as in Example 2, except that a methyl methacrylate-styrene copolymer MS-750 (manufactured by Toyo Styrene) having a styrene-derived structural unit content of 25% by weight was used instead of KT-89 (manufactured by Denka), and the raw film was simultaneously biaxially stretched at a temperature 10°C higher than the glass transition temperature of the acrylic resin composition. At this time, the acrylic resin composition had a glass transition temperature of 122°C, a 1% weight loss temperature of 306°C, an Mw of 76,000, and an Mw / Mn of 1.59.

[0090] Example 5 A polarizer protective film was obtained in the same manner as in Example 4, except that 10 wt% of methyl methacrylate resin Parapet HM (manufactured by Kuraray) was added instead of KT-89 (manufactured by Denka). The acrylic resin composition had a glass transition temperature of 120°C, a 1% weight loss temperature of 302°C, an Mw of 81,000, and an Mw / Mn of 1.59.

[0091] Comparative Example 1 A polarizer protective film was obtained in the same manner as in Example 1, except that KT-89 (manufactured by Denka) was not used. The acrylic resin composition had a glass transition temperature of 123°C and a 1% weight loss temperature of 310°C.

[0092] Comparative Example 2 A polarizer protective film was obtained in the same manner as in Comparative Example 1, except that acrylic resin 2 was used instead of acrylic resin 1. In this case, the acrylic resin composition had a glass transition temperature of 125°C and a 1% weight loss temperature of 315°C.

[0093] Comparative Example 3 A polarizer protective film was obtained in the same manner as in Example 1, except that the acrylic resin 1 was not used and the raw film was simultaneously biaxially stretched at a temperature 20°C higher than the glass transition temperature of the acrylic resin composition. At this time, the acrylic resin composition had a glass transition temperature of 117°C and a 1% weight loss temperature of 297°C.

[0094] Comparative Example 4 A polarizer protective film was obtained in the same manner as in Comparative Example 3, except that a methyl methacrylate-styrene copolymer MS800 (manufactured by Nippon Steel Chemical Co., Ltd.) having a styrene-derived structural unit content of 20% by weight was used instead of KT-89 (manufactured by Denka Chemical Co., Ltd.), and the raw film was simultaneously biaxially stretched at a temperature 30°C higher than the glass transition temperature of the acrylic resin composition. In this case, the acrylic resin composition had a glass transition temperature of 115°C and a 1% weight loss temperature of 296°C.

[0095] Comparative Example 5 A polarizer protective film was obtained in the same manner as in Comparative Example 1, except that acrylic resin 3 was used instead of acrylic resin 1, and the raw film was simultaneously biaxially stretched at a temperature 35°C higher than the glass transition temperature of the acrylic resin composition. In this case, the acrylic resin composition had a glass transition temperature of 125°C and a 1% weight loss temperature of 320°C.

[0096] Table 2 shows the properties and evaluation results of the acrylic resin composition and the polarizer protective film.

[0097]

[0098] Table 2 shows that the polarizer protective films of Examples 1 to 5 achieve both a reduced standard deviation of Re and a reduced YI when viewed obliquely from the liquid crystal panel. In contrast, the polarizer protective film of Comparative Example 1 has a Δnxy of 0.0 and an Rth of 0.0 nm, and therefore exhibits a large YI when viewed obliquely from the liquid crystal panel. The polarizer protective film of Comparative Example 2 has a Δnxy of 4.0×10 -4 , and Rth is 10.2 nm, so that YI is large when viewed from an oblique direction of the liquid crystal panel. -3 , −2.5×10 -3 , −3.3 × 10 -3 Therefore, the standard deviation of Re becomes large.

Claims

1. An optical film comprising an acrylic resin composition, the thickness direction retardation Rth at a wavelength of 590 nm being −15.0 nm or more and less than 0.0 nm, the acrylic resin composition comprising an acrylic resin having a ring structure in the main chain, a glass transition temperature of 120° C. or more, and a birefringence expression Δnxy of −1.0×10 -3 Above -0.1 x 10 -3 The polarizer protection film is as follows.

2. The polarizer protective film according to claim 1, wherein the acrylic resin having a ring structure in its main chain has a structural unit containing in its main chain one or more ring structures selected from the group consisting of a glutarimide ring, a lactone ring, a maleic anhydride ring, a maleimide ring and a glutaric anhydride ring.

3. The polarizer protective film according to claim 2, wherein the acrylic resin having a ring structure in its main chain has a structural unit represented by the following formula (1): (In the formula, R 1 and R 2 are each independently a hydrogen atom or an alkyl group having 1 to 8 carbon atoms; R 3 is a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, or a cycloalkyl group having 3 to 12 carbon atoms.

4. The polarizer protective film according to claim 1, wherein the acrylic resin composition has a content of structural units derived from aromatic vinyl of 0% by weight or more and 8% by weight or less.

5. The polarizer protective film according to claim 4, wherein the acrylic resin composition has a content of structural units derived from styrene of 0% by weight or more and 8% by weight or less.

6. The polarizer protective film according to claim 1, wherein the acrylic resin composition further contains polymethyl methacrylate or a methyl methacrylate-styrene copolymer.

7. The polarizer protective film according to claim 1, wherein the acrylic resin composition has a 1% weight loss temperature of 300° C. or higher.

8. The polarizer protective film according to claim 1, which does not contain an ultraviolet absorber.

9. The polarizer protective film according to claim 1, which is a biaxially stretched film.

10. The polarizer protective film according to claim 1, having a yellowness index of 0.01 or more and 5.00 or less.

11. The polarizer protective film according to claim 1, which has an absorbance at a wavelength of 380 nm of 0.01 or more and 1.00 or less.

12. The polarizer protective film according to claim 1, wherein the absolute value of the Nz coefficient is 0.1 or more and 30.0 or less, the ratio Rth(447) / Rth(548) of the thickness direction retardation Rth(447) at a wavelength of 447 nm to the thickness direction retardation Rth(548) at a wavelength of 548 nm is 0.50 or more and 1.10 or less, and the ratio Rth(628) / Rth(548) of the thickness direction retardation Rth(628) at a wavelength of 628 nm to the thickness direction retardation Rth(548) at a wavelength of 548 nm is 0.50 or more and 2.00 or less.

13. A polarizing plate comprising the polarizer protective film according to any one of claims 1 to 12.

14. A liquid crystal panel comprising the polarizing plate according to claim 13.

Citation Information

Patent Citations

  • Coating film for optical compensation, optical element and manufacturing method of coating film for optical compensation

    JP2009251530A

  • Optical compensation film and method of manufacturing the same

    JP2009276695A

  • Resin composition, and film thereof

    JP2015214713A

  • Method for producing optical film and optical film

    JP2019105819A