Magnetic memory element, magnetic memory device, and photonic spin register

Antiferromagnetic materials with specific microstructures are used in magnetic memory elements and photonic spin registers to achieve faster operation and efficient data handling, addressing the speed limitations of ferromagnetic MRAM by leveraging their faster spin response and optical signal manipulation capabilities.

WO2024204298A1PCT designated stage expired Publication Date: 2024-10-03THE UNIV OF TOKYO

Patent Information

Application Number
PCT/JP2024/012153
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current magnetic random access memory (MRAM) using ferromagnetic materials has limitations in magnetization reversal speed, unable to respond in the THz band, while antiferromagnetic materials offer faster spin response speeds but have unknown applications in nanometer-order magnetic memory elements.

Method used

A magnetic memory element utilizing an antiferromagnetic material with a microstructure of second grains within nanoscale first grains, exhibiting the anomalous Hall effect, and a photonic spin register that reverses magnetic order using optical signals, enabling high-speed operation.

Benefits of technology

The use of antiferromagnetic materials in magnetic memory elements achieves faster spin response speeds and high integration potential, with the photonic spin register allowing for efficient data writing and reading using optical signals, overcoming the speed limitations of ferromagnetic MRAM.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012153_03102024_PF_FP_ABST
    Figure JP2024012153_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A magnetic memory element (100) is provided with an antiferromagnetic layer (14) and a spin Hall layer (12). The antiferromagnetic layer (14) is a polycrystalline thin film which is made of an antiferromagnetic material exhibiting an anomalous Hall effect, and has one or a plurality of first grains having an average particle diameter in the range of 20-200 nm, with a plurality of second grains present inside each of the first grains. The spin Hall layer (12) is in contact with the antiferromagnetic layer (14) and is made of a material exhibiting a spin Hall effect, wherein, when a write current Iwrite flows in the in-plane direction, a spin flow is generated in a direction perpendicular to the plane. In the antiferromagnetic layer (14), the spin orbit torque generated by the spin flow acts on the magnetic order of the antiferromagnetic material so that the magnetic order can be reversed.
Need to check novelty before this filing date? Find Prior Art

Description

Magnetic memory element, magnetic memory device, and photonic spin register

[0001] The present invention relates to a magnetic memory element, a magnetic memory device, and a photonic spin register.

[0002] Magnetic random access memory (MRAM) using ferromagnetic materials is attracting attention as a nonvolatile memory that can realize low-power information processing. In fact, various semiconductor manufacturers have adopted MRAM as a replacement for volatile memory such as static random access memory (SRAM). Examples of such MRAM include STT-MRAM, which uses spin-transfer torque (STT) to reverse the magnetization of a ferromagnetic material, and SOT-MRAM, which uses spin-orbit torque (SOT) to reverse the magnetization of a ferromagnetic material (see, for example, Patent Document 1).

[0003] U.S. Patent No. 9,837,602

[0004] However, because current MRAMs use ferromagnetic materials, their magnetization reversal speed is limited to approximately 1 nanosecond, making them unable to support the terahertz (picosecond) range, which will become increasingly important as optical communication speeds increase. Antiferromagnetic materials, on the other hand, have a faster spin response speed than ferromagnetic materials and are expected to be used as materials for magnetic memory elements capable of high-speed operation. While antiferromagnetic materials have been studied for their potential as spintronics materials in thin films with large size scales, their application to actual magnetic memory elements on the nanometer order remains unknown.

[0005] The present invention has been made in view of the above-mentioned problems, and has an object to make it possible to realize a magnetic memory element using an antiferromagnetic material.

[0006] A magnetic memory element according to a first aspect of the present invention comprises an antiferromagnetic material that exhibits an anomalous Hall effect, has one or more first grains with an average grain size in the range of 20 nm to 200 nm, and is provided with a polycrystalline antiferromagnetic layer in which a plurality of second grains exist within each first grain, and the magnetic order of the antiferromagnetic material is reversible.

[0007] A magnetic memory device according to a second aspect of the present invention includes a plurality of magnetic memory elements, each of which is defined as a magnetic memory element including the above-described antiferromagnetic layer.

[0008] A photonic spin register according to a third aspect of the present invention includes the above-described magnetic memory element and a photodetector that receives a pulse-amplitude-modulated optical signal and converts it into a photocurrent. When a photocurrent flows in the in-plane direction as a write current in the spin Hall layer, a spin current is generated in the perpendicular direction.

[0009] A photonic spin register according to a fourth aspect of the present invention includes the above-described magnetic memory element and a light irradiation unit that irradiates an antiferromagnetic layer with a pulse-amplitude-modulated optical signal, whereby the magnetic order of the antiferromagnetic material can be reversed by irradiation with the optical signal.

[0010] According to the present invention, it is possible to realize a magnetic memory element using an antiferromagnetic material having a microstructure in which a second grain exists inside a nanoscale first grain.

[0011] Mn 3 FIG. 1 is a perspective view of the crystal structure and spin structure of Sn. 3 A plan view of the crystal structure and spin structure of Sn. 3 1 is a graph showing the X-ray diffraction spectrum of Sn. 3 Atomic force microscope (AFM) images a to d of the Sn sample and Mn samples with film thicknesses of 25 nm and 20 nm. 3 e and f are cross-sectional transmission electron microscope (TEM) images of the Sn sample. Schematic diagram of Hall effect measurement. 3 1 is a graph showing the magnetic field dependence of the Hall resistivity of a Sn sample. 3 1 is a graph showing the magnetic field dependence of Hall resistivity when an Al layer with a thickness of 4 nm is formed on a Sn sample. 3 1 is a graph showing the magnetic field dependence of the normalized Hall resistivity, obtained by dividing the Hall resistivity by its respective saturation value, for Sn samples. 3This is a schematic diagram showing the state in which isolated grains of Sn are electrically insulated from each other. 3 FIG. 1 is a schematic diagram showing a conduction state in which isolated grains of Sn are electrically connected. FIG. 2 is a schematic diagram showing the configuration of a magnetic memory element with a Hall bar structure according to Example 1. FIG. 3 is a schematic diagram showing the configuration of a magnetic memory element of an SOT-MRAM according to Example 2. FIG. 4 is a schematic diagram showing the configuration of a magnetic memory element of an STT-MRAM according to Example 3. FIG. 5 is a schematic diagram showing the configuration of a photonic spin register according to Example 4. FIG. 6 is a schematic diagram showing the configuration of a photonic spin register according to Example 6.

[0012] Hereinafter, embodiments of the present invention will be described with reference to the drawings. In the following embodiments, the same or similar components are designated by the same reference numerals throughout the drawings. The drawings are schematic, and the relationship between planar dimensions and thickness, and the thickness ratio of each component, differ from the actual ones. Furthermore, it goes without saying that the dimensional relationships and ratios of each component differ between the drawings.

[0013] In this embodiment, an antiferromagnetic material is used instead of a ferromagnetic material to realize a nonvolatile memory that can operate at high speed. The reason is that the spin response speed of an antiferromagnetic material is in the THz range (picoseconds), which is two to three orders of magnitude faster than that of a ferromagnetic material, and the interaction between magnetic materials is small, so there is a possibility that magnetic devices can be made even faster and more highly integrated.

[0014] In this embodiment, the object is particularly an antiferromagnetic material that has an antiferromagnetic order in which time reversal symmetry is broken macroscopically and that exhibits the anomalous Hall effect. Examples of such antiferromagnetic materials include antiferromagnetic metals containing manganese (Mn) and collinear antiferromagnetic materials (e.g., RuO 2 , Mn 5 Si 3 Examples of antiferromagnetic metals containing Mn include Mn 3 X (X=Sn, Ge, Ga, Rh, Pt, Ir), Mn 3XN (X=Ga, Sn, Ni), gamma-type Mn alloys with a face-centered cubic (fcc) structure are listed. 1-x Fe x , Mn 1-x Rh x , Mn 1-x Pd x Examples include:

[0015] 1A and 1B, Mn is an example of an antiferromagnetic material that exhibits the anomalous Hall effect. 3 The characteristics of Sn will be explained.

[0016] Mn 3 Sn is an antiferromagnetic material with a triangular crystal structure called the kagome lattice. As shown in Figures 1A and 1B, the kagome lattice is stacked along the c-axis

[0001] . Due to geometric frustration, Mn atoms located at the vertices of the kagome lattice possess a non-collinear chiral spin structure at temperatures below 420 K, in which the magnetic moments (localized spin orientations) are inclined 120 degrees relative to each other. Three types of six-spin units arranged on a bilayer kagome lattice form a spin order called a cluster magnetic octupole, represented by a hexagon. This non-collinear magnetic structure can be regarded as a ferromagnetic order of the cluster magnetic octupole. This ferromagnetic order breaks time-reversal symmetry macroscopically.

[0017] The cluster magnetic octopole corresponds to the orientation of Weyl points, which are topological electronic structures, and the virtual magnetic field in momentum space (equivalent to 100-1000 Tesla (T) in real space), and the response derived from the Weyl points and the virtual magnetic field can be controlled by the orientation of the cluster magnetic octopole.

[0018] The magnetic structure shown in Figures 1A and 1B has orthorhombic symmetry, and only one of the three magnetic moments of Mn located at the vertices of the triangle is parallel to the easy axis of magnetization. The other two magnetic moments are canted with respect to the easy axis of magnetization, which is thought to induce a weak ferromagnetic moment. An antiferromagnet with a canted magnetic moment and thus a small magnetization is called a canted antiferromagnet.

[0019] Mn 3 The Sn sample can be prepared by DC magnetron sputtering. For example, the base pressure is <5×10 -7 In a chamber at 60 Pa, Mn was deposited under the conditions of a sputtering power of 60 W and an Ar pressure of 0.7 Pa. 2.7 Mn was deposited from a Sn target onto a thermally oxidized Si substrate at a high temperature of 500°C. 3 A Sn film is formed. 3 Immediately after the Sn film is formed, it is cooled to room temperature. Then, to prevent oxidation, Mn 3 A cap layer (thickness: 2 nm) made of aluminum (Al) is formed on the Sn film at room temperature. 3 The method for preparing the Sn sample is not limited to the above-mentioned method, and other preparation methods can also be adopted.

[0020] Mn 3 The crystalline structure of the Sn film can be investigated using X-ray diffraction. 2 Mn film deposited on the substrate at 500°C 3 The X-ray diffraction spectrum of the 2θ / ω scan at room temperature for the Sn film (film thickness t = 40 nm) is shown. 19 Type Mn 3 1 shows a simulated diffraction pattern for Sn.

[0021] The X-ray diffraction spectrum obtained by 2θ / ω scanning is 19 Type Mn 3 Sn and Si / SiO 2 Since the peaks are the same as those of the substrate, Mn 3 The Sn film is D0 19 Type Mn3 It can be seen that the sample is a single phase of Sn. The peak intensity ratio is also in close agreement with the simulation results. These results indicate that the sample is composed of Mn 3 This indicates that the Sn film is polycrystalline, with crystals of various orientations mixed together. Here, the lattice constants are estimated to be a = 5.66 Å and c = 4.51 Å.

[0022] Mn 3 To clarify the structural characteristics of the Sn film, Fig. 3 shows the Mn 3 Atomic force microscope (AFM) images a to d of Sn samples and Mn samples with t = 25 nm and t = 20 nm. 3 Cross-sectional transmission electron microscope (TEM) images e and f of the Sn sample are shown.

[0023] TEM image e shows that the sample with t = 25 nm has a continuous structure, although there are slight irregularities on the surface. On the other hand, TEM image f shows that the sample with t = 20 nm has a discontinuous surface with an isolated island structure. In other words, the sample with t ≥ 25 nm is conductive due to its continuous structure, while the sample with t ≤ 20 nm is electrically insulating due to its discontinuous structure.

[0024] Furthermore, AFM image c shows that the sample with t = 20 nm has multiple grains with relatively large grain sizes (hereinafter referred to as "first grains"), and each first grain has multiple grains with relatively small grain sizes (hereinafter referred to as "second grains"). The average grain size of the first grains in the sample with t = 20 nm is approximately 100 nm. In contrast, AFM image d shows that the sample with t = 5 nm has many first grains with grain sizes less than 20 nm, but no second grains within them.

[0025] From the AFM images c and d and the TEM image f, it can be seen that the average particle size of the first grains is in the range of 20 nm to 200 nm, and that within the first grains there are multiple second grains whose average particle size is 1 / 2 or less of that of the first grains, more specifically in the range of 1 / 20 to 1 / 2.

[0026] Next, the Hall effect measurement for the antiferromagnetic material of this embodiment will be described with reference to FIGS. 4 to 6B.

[0027] As shown in FIG. 4, in the Hall effect measurement, when a magnetic field H is applied in the direction perpendicular to the surface of the antiferromagnetic layer 2 (z direction) and a current I is passed in the longitudinal direction (x direction), a Hall voltage V is generated in the y direction perpendicular to both the current I and the magnetic field H. y The length of the antiferromagnetic layer 2 in the x direction is l, the width in the y direction is w, and the film thickness in the z direction is t. The longitudinal voltage in the x direction is V x When written as such, the longitudinal resistivity ρ xx and Hall resistivity ρ yx are respectively (V x / I)・(wt / l), (V y / I)·t.

[0028] FIG. 5A shows the Mn 3 Hall resistivity ρ of the Sn sample (antiferromagnetic layer 2) yx As shown in Figure 5A, a clear hysteresis loop appears, and ρ yx The magnitude of the magnetic field is about 1.3 μΩcm, and the coercive force is about 0.6 T. 3 The anomalous Hall effect appears in the Sn sample.

[0029] t=20 nm Mn 3 The Sn sample has a discontinuous surface structure as shown in the TEM image f of Fig. 3. In this case, as shown in Fig. 6A, Mn 3 An antiferromagnetic layer 2 having a plurality of isolated grains made of Sn is deposited, and these isolated grains are covered with a 2 nm thick Al cap layer. This cap layer is oxidized to form an oxide film 3, which electrically insulates the isolated grains. In this insulating state, the Hall effect cannot be measured.

[0030] 6B , by increasing the thickness of the cap layer, a part of the cap layer remains as the conductive layer 4, and the isolated grains are electrically connected via the conductive layer 4. For example, if the thickness of the Al cap layer is set to 4 nm, the surface 2 nm becomes the oxide film 3, but the remaining 2 nm on the antiferromagnetic layer 2 and substrate 1 side remains as the conductive layer 4.

[0031] FIG. 5B shows the Mn 3 Hall resistivity ρ at 300 K when the Sn sample (antiferromagnetic layer 2) was covered with a 4 nm thick Al cap layer yx The conductive layer 4 in FIG. 6B not only electrically connects the isolated grains but also induces a large shunt effect, so that the Hall voltage V y In fact, as shown in FIG. 5B, ρ yx The magnitude of ρ is about 0.06 μΩcm, and the ρ of the sample with t = 40 nm yx 5B indicates that the normal Hall effect of the Al conductive layer 4 is manifested.

[0032] FIG. 5C shows the Mn 3 For the Sn sample, the Hall resistivity ρ at 300 K yx Figure 5C shows the magnetic field dependence of the normalized Hall resistivity, obtained by subtracting the component linearly proportional to the magnetic field and then dividing by the respective saturation values. This normalization subtracts the contribution of the normal Hall effect, allowing the two samples to be compared independently of the shunt effect. Figure 5C shows that both samples exhibit nearly identical hysteresis loops.

[0033] t=5 nm Mn 3In the Hall effect measurement of the Sn sample, only the normal Hall effect was observed. That is, the anomalous Hall effect was not observed in the sample with t = 5 nm, which does not have a second grain, but the anomalous Hall effect was observed in the sample with t = 20 nm, which has a second grain within the first grain (FIGS. 5B and 5C). From this, it can be inferred that the presence of the second grain within the first grain causes the anomalous Hall effect to appear even in very small grains with a particle size of 20 nm to 200 nm.

[0034] As described above, the antiferromagnetic material targeted in this embodiment has a characteristic nanoscale microstructure and exhibits a stable magnetic effect, making it applicable to magnetic memory elements.

[0035] Next, Examples 1 to 6 of magnetic memory elements having the above-described antiferromagnetic layer will be described with reference to Figures 7 to 12. Example 1 focuses on a magnetic memory element with a Hall bar structure (see Figure 7), Examples 2 and 3 focus on a magnetic memory element having a magnetoresistive element (see Figures 8 and 9), and Examples 4 to 6 focus on a photonic spin register capable of writing data corresponding to an optical signal (see Figures 10 to 12). In each example, one or more first grains correspond to one bit of information.

[0036] 7 shows the configuration of a magnetic memory element 100 according to Example 1. The magnetic memory element 100 includes a substrate 10, a spin Hall layer 12 stacked on the substrate 10, and an antiferromagnetic layer 14 in contact with the spin Hall layer 12.

[0037] The substrate 10 is made of MgO, SiO 2The spin Hall layer 12 is made of an insulator such as tantalum (Ta), tungsten (W), platinum (Pt), or another non-magnetic heavy metal, or a chalcogenide material such as a topological insulator. The antiferromagnetic layer 14 is a polycrystalline thin film of an antiferromagnetic material that exhibits the anomalous Hall effect as described above, and has one or more first grains with an average grain size in the range of 20 nm to 200 nm. Within each first grain, there are multiple second grains with an average grain size equal to or less than half that of the first grain. In particular, it is more desirable for the average grain size of the second grains to be in the range of 1 / 20 to 1 / 2 of that of the first grain.

[0038] Electrodes 16a and 16b are arranged at both ends in the longitudinal direction (x direction) of the magnetic memory element 100, and electrodes 18a and 18b are arranged in the lateral direction (y direction) of the magnetic memory element 100. For example, the electrodes 16a and 16b and the electrodes 18a and 18b are made of Au / Ti.

[0039] When writing data to the magnetic memory element 100, a write current I is applied to the spin Hall layer 12 between the electrodes 16a and 16b. write A pulse current (pulse current) is passed in the x direction. This generates a spin current in the perpendicular direction (z direction) due to the spin Hall effect, and spin-orbit torque (SOT) acts on the magnetic order (magnetization) of the antiferromagnetic layer 14, reversing the magnetic order. At this time, by applying a weak bias magnetic field in the x direction, the magnetic order of the antiferromagnetic layer 14 is affected by the bias magnetic field, and the direction of rotation of the magnetic order is determined.

[0040] In this way, data ("0" or "1") can be written to the antiferromagnetic layer 14. The write current I write The direction of the magnetic order of the antiferromagnetic layer 14 can be controlled by the direction of the write current I write When a write current I flows in the -x direction, the magnetic order is reversed from the +z direction ("1") to the -z direction ("0"). write When a current is applied, the magnetic order is reversed from the −z direction (“0”) to the +z direction (“1”).

[0041] When reading data stored in the antiferromagnetic layer 14, a read current I is applied to the antiferromagnetic layer 14 between the electrodes 16a and 16b. read (direct current) flows in the x direction. As a result, a Hall voltage V H The Hall voltage V H The sign of is determined by the z-component of the magnetic order of the antiferromagnetic layer 14. For example, when the magnetic order of the antiferromagnetic layer 14 is oriented in the +z direction, it corresponds to "1," and when it is oriented in the -z direction, it corresponds to "0."

[0042] 7, a configuration (substrate / antiferromagnetic layer / spin Hall layer) in which the spin Hall layer 12 is stacked on the antiferromagnetic layer 14 may be employed. Also, the antiferromagnetic layer 14 may be sandwiched between two spin Hall layers made of spin Hall materials having spin Hall angles of different signs.

[0043] 8 shows the configuration of a magnetic memory element 200 of an SOT-MRAM according to Example 2. The magnetic memory element 200 includes a magnetoresistive element 210, a spin Hall layer 220, a first terminal 231, a second terminal 232, a third terminal 233, and transistors Tr1 and Tr2.

[0044] The spin Hall layer 220 is made of a spin Hall material, similar to the spin Hall layer 12 in Fig. 7. The magnetoresistive element 210 is in contact with the spin Hall layer 220 and includes a free layer 212, which is an antiferromagnetic layer whose magnetic order (magnetization) is reversible, a non-magnetic layer 214 stacked on the free layer 212, and a reference layer 216 stacked on the non-magnetic layer 214, whose magnetic order is fixed in the in-plane or perpendicular to the plane. Fig. 8 shows the case where the magnetic orders of the free layer 212 and the reference layer 216 are oriented in the perpendicular to the plane.

[0045] The free layer 212 is made of an antiferromagnetic material that exhibits the anomalous Hall effect, similar to the antiferromagnetic layer 14 of FIG. 7. The nonmagnetic layer 34 is made of an insulator (e.g., MgO, AlOx, or MgAl 2 O 4). The reference layer 216 is made of a ferromagnetic material (e.g., CoFeB). The reference layer 216 may be made of the same antiferromagnetic material as the free layer 212, in which case the antiferromagnetic material of the reference layer 216 has a greater coercive force than the antiferromagnetic material of the free layer 212. The magnetoresistive element 210 functions as a magnetic tunnel junction (MTJ) element.

[0046] The magnetoresistive element 210 is assigned one bit of data, either "0" or "1," depending on the resistance state. For example, when the free layer 212 and the reference layer 216 are made of Mn 3 In the case of Sn, when the magnetic order of the cluster magnetic octopoles in the reference layer 216 and the free layer 212 is in the same direction (parallel state), the magnetoresistive element 210 is in a low resistance state, and when the magnetic order is in the opposite direction (antiparallel state), the magnetoresistive element 210 is in a high resistance state. For example, data in the parallel state can be assigned as "0," and data in the antiparallel state can be assigned as "1." Experiments have shown that the magnetoresistive element 210 can be in a high resistance state in the parallel state and in a low resistance state in the antiparallel state.

[0047] The first terminal 231, the second terminal 232, and the third terminal 233 are made of metal. The first terminal 231 is connected to the reference layer 216, the second terminal 232 is connected to one end of the spin Hall layer 220, and the third terminal 233 is connected to the other end of the spin Hall layer 220. The first terminal 231 is connected to a ground line 240. The ground line 240 is set to the ground voltage. Note that the ground line 240 may be set to a reference voltage other than the ground voltage.

[0048] The transistors Tr1 and Tr2 are, for example, N-channel metal oxide semiconductor (NMOS) transistors. The second terminal 232 is connected to the drain of the transistor Tr1, and the third terminal 233 is connected to the drain of the transistor Tr2. The gates of the transistors Tr1 and Tr2 are connected to the word line WL. The source of the transistor Tr1 is connected to the first bit line BL1, and the source of the transistor Tr2 is connected to the second bit line BL2.

[0049] As shown in FIG. 8, when the magnetic order of the free layer 212 and the reference layer 216 is oriented in the perpendicular direction, a write current I write A weak bias magnetic field is applied in the direction of the arrow A, the word line WL is set to a high level to turn on the transistors Tr1 and Tr2, and one of the first bit line BL1 and the second bit line BL2 is set to a high level and the other is set to a low level. As a result, a write current I flows in the in-plane direction of the spin Hall layer 220 between the first bit line BL1 and the second bit line BL2. write The flow of the write current I generates a spin current in the perpendicular direction, and the magnetic order of the free layer 212 is reversed by the SOT, allowing data to be written. write The data to be written can be changed depending on the direction of the

[0050] When reading data stored in the magnetoresistive element 210, the word line WL is set to a high level to turn on the transistors Tr1 and Tr2, one bit line (the second bit line BL2) is set to a high level, and the other bit line (the first bit line BL1) is set to an open state. As a result, a read current I flows from the high-level second bit line BL2 to the third terminal 233, the spin Hall layer 220, the free layer 212, the nonmagnetic layer 214, the reference layer 216, the first terminal 231, and the ground line 240. read The read current I read By measuring the magnitude of the potential difference, the resistance state of the magnetoresistive element 210, that is, the stored data, can be determined.

[0051] 9 shows the configuration of a magnetic memory element 300 of an STT-MRAM according to Example 3. The magnetic memory element 300 includes a magnetoresistive element 310, a first terminal 321, a second terminal 322, and a transistor Tr.

[0052] The magnetoresistive element 310 includes a reference layer 316 whose magnetic order is fixed in the in-plane or perpendicular direction, a non-magnetic layer 314 stacked on the reference layer 316, and a free layer 312 stacked on the non-magnetic layer 314 as an antiferromagnetic layer whose magnetic order is reversible. The free layer 312, the non-magnetic layer 314, and the reference layer 316 are made of the same materials as the free layer 212, the non-magnetic layer 214, and the reference layer 216 in FIG. 8, respectively. FIG. 9 shows a case where the magnetic orders of the free layer 312 and the reference layer 316 are oriented in the perpendicular direction. Similar to the magnetoresistive element 210 in FIG. 8, one bit of data, "0" or "1," is assigned to the magnetoresistive element 310 depending on the resistance state.

[0053] The first terminal 321 and the second terminal 322 are made of metal. The free layer 312 is connected to the first terminal 321, and the reference layer 316 is connected to the second terminal 322. The first terminal 321 is connected to the bit line BL, and the second terminal 322 is connected to the transistor Tr.

[0054] The transistor Tr is, for example, an NMOS transistor. The drain of the transistor Tr is connected to the second terminal 322, the source is connected to a source line SL, and the gate is connected to a word line WL.

[0055] When writing data to the magnetoresistive element 310, the word line WL is set to a high level to turn on the transistor Tr, and a write current I flows perpendicular to the surface between the bit line BL and the source line SL. write This causes the magnetic order of the free layer 312 to be reversed by the spin transfer torque, allowing data to be written. write The data to be written can be changed depending on the direction of the

[0056] When reading data stored in the magnetoresistive element 310, the word line WL is set to a high level to turn on the transistor Tr, and a read current I read The read current I read By measuring the magnitude of the potential difference, the resistance state of the magnetoresistive element 310, that is, the stored data, can be determined.

[0057] Although the magnetoresistive elements 210 and 310 are MTJ elements in the second embodiment (FIG. 8) and the third embodiment (FIG. 9), they may also function as giant magnetoresistive (GMR) elements. In this case, the nonmagnetic layers 214 and 314 are made of a nonmagnetic metal (conductor).

[0058] Furthermore, in Example 2 (FIG. 8), a structure (antiferromagnetic layer / ferromagnetic layer) in which a very thin ferromagnetic layer (e.g., CoFeB) of 1 nm or less is stacked on an antiferromagnetic layer may be used as the free layer 212, and a magnetoresistive element consisting of an antiferromagnetic layer / ferromagnetic layer / non-magnetic layer / reference layer may be employed. By inverting this stacked structure, a magnetoresistive element consisting of a reference layer / non-magnetic layer / ferromagnetic layer / antiferromagnetic layer may be employed in Example 3 (FIG. 9). In this way, when an antiferromagnetic layer and a very thin ferromagnetic layer are magnetically coupled, high-speed control comparable to that of an antiferromagnetic material is possible, and the spin polarization of the ferromagnetic material can be utilized, which is expected to enable high-speed memory.

[0059] 10 shows the configuration of a photonic spin register 400 according to Example 4. The photonic spin register 400 includes an optical receiver 410 and a magnetic memory element 420.

[0060] The magnetic memory element 420 includes a spin Hall layer 430 and an antiferromagnetic layer 440 in contact with the spin Hall layer 430 and having a reversible magnetic order (magnetization). The spin Hall layer 430 is made of a spin Hall material, similar to the spin Hall layer 12 in Fig. 7. The antiferromagnetic layer 440 is made of an antiferromagnetic material that exhibits the anomalous Hall effect, similar to the antiferromagnetic layer 14 in Fig. 7.

[0061] The optical receiver 410 includes an optical waveguide 412 provided on a substrate, and a photodetector 414 connected to the optical waveguide 412 on the substrate. The photodetector 414 includes a photoelectric conversion element 416, and a first metal film 418a and a second metal film 418b that sandwich the photoelectric conversion element 416, and constitutes a plasmon waveguide.

[0062] The photoelectric conversion element 416 is made of a dielectric (semiconductor or insulator) and is continuously connected to the optical waveguide 412. The width of the photoelectric conversion element 416 is narrower than the width of the optical waveguide 412, and the optical waveguide 412 has a tapered shape where the connection portion with the photoelectric conversion element 416 narrows toward the photoelectric conversion element 416. The narrower the width of the photoelectric conversion element 416, the greater the light confinement effect, making it possible to focus light below the diffraction limit, and strengthening the interaction between the photoelectric conversion element 416 and the optical electric field.

[0063] The first metal film 418a and the second metal film 418b are made of a metal such as Au or Ag. The second metal film 418b is connected to one end of the spin Hall layer 430. The first metal film 418a also functions as an electrode, to which a bias voltage is applied. The other end of the spin Hall layer 430 is connected to an electrode 450, which is grounded.

[0064] Next, an operation of writing data corresponding to the optical signal PL to the magnetic memory element 420 will be described. When the serially input pulse amplitude modulated optical signal PL is input to the photoelectric conversion element 416 via the optical waveguide 412, the optical signal PL propagates as surface plasmon polaritons at the interfaces between the photoelectric conversion element 416 and the first and second metal films 418a and 418b, generating a strong electric field in the vicinity. At this time, application of a bias voltage causes a pulse current, a photocurrent I, to flow from the photodetector 414 to the spin Hall layer 430. ph flows and flows into electrode 450.

[0065] Photocurrent I as a write current to the spin Hall layer 430 ph When the photocurrent I flows in the in-plane direction, a spin current is generated in the spin Hall layer 430 in the perpendicular direction, and the SOT acts on the magnetic order of the antiferromagnetic layer 440, thereby reversing the magnetic order. In this way, data corresponding to the optical signal PL can be written in the antiferromagnetic layer 440. Here, the photocurrent I ph is a pulse current corresponding to the optical signal PL, the magnetic order is reversed during the pulse width period when a current with a current density equal to or greater than a predetermined value flows, and the magnetic order is not reversed during other periods.

[0066] When reading data stored in the antiferromagnetic layer 440, a photocurrent I ph A read current (DC) is passed in the same direction as the read current, which generates a Hall voltage in a direction perpendicular to the read current due to the anomalous Hall effect, and the Hall voltage is detected between terminals 442 a and 442 b of the antiferromagnetic layer 440.

[0067] In this way, the photonic spin register 400 generates a photocurrent I from the photodetector 414. ph The magnetic order of the antiferromagnetic layer 440 can be reversed by the above method, and a high-speed optical / electrical interface utilizing spintronics can be realized.

[0068] 11 shows the configuration of a photonic spin register 500 according to Example 5. The photonic spin register 500 includes an optical receiver 410 and a magnetic memory element 520. The photonic spin register 500 has the same configuration as the photonic spin register 400 shown in FIG. 10 , except that the magnetic memory element 420 is replaced with the magnetic memory element 520.

[0069] The magnetic memory element 520 includes a spin Hall layer 530 and a magnetoresistive element 540 stacked on the spin Hall layer 530 .

[0070] The spin Hall layer 530 is made of a spin Hall material, similar to the spin Hall layer 12 in Fig. 7. One end of the spin Hall layer 530 is connected to the second metal film 418b of the optical receiver 414, and the other end is connected to the electrode 450.

[0071] The magnetoresistive element 540 is in contact with the spin Hall layer 530 and includes a free layer 542, which is an antiferromagnetic layer whose magnetic order (magnetization) is reversible, a nonmagnetic layer 544 stacked on the free layer 542, and a reference layer 546 stacked on the nonmagnetic layer 544 and whose magnetic order is fixed in the in-plane or perpendicular-to-plane direction. The free layer 542, the nonmagnetic layer 544, and the reference layer 546 are made of the same materials as the free layer 212, the nonmagnetic layer 214, and the reference layer 216 in FIG. 8, respectively. The reference layer 546 is connected to a terminal 551.

[0072] When data corresponding to the pulse amplitude modulated optical signal PL is written to the magnetic memory element 520, the photocurrent I corresponding to the optical signal PL is ph The flow of spin current in the in-plane direction of the spin Hall layer 530 generates a spin current in the perpendicular direction, and the SOT reverses the magnetic order of the free layer 542. This allows data corresponding to the optical signal PL to be written in the magnetoresistive element 540.

[0073] When reading data stored in the magnetoresistive element 540, a read current is passed in the direction perpendicular to the surface from the spin Hall layer 530 side toward the magnetoresistive element 540. By measuring the magnitude of the read current via the terminal 551, the resistance state of the magnetoresistive element 540, i.e., the stored data, can be determined.

[0074] In this way, the photonic spin register 500 detects the photocurrent I from the photodetector 414. ph The magnetic order of the free layer 542 can be reversed by the spintronics technique, and a high-speed optical / electrical interface can be realized.

[0075] Example 6 deals with a photonic spin register that utilizes all-optical magnetization switching (AOS), which reverses the magnetic order (magnetization) by irradiating an optical signal onto an antiferromagnetic layer.

[0076] 12 shows the configuration of a photonic spin register 600 according to Example 6. The photonic spin register 600 includes a light irradiating unit 610 and an antiferromagnetic layer 620 as a magnetic memory element.

[0077] The antiferromagnetic layer 620 is made of an antiferromagnetic material that exhibits the anomalous Hall effect, similar to the antiferromagnetic layer 14 in FIG.

[0078] The light emitting unit 610 includes a light output unit 612 and a lens 614. The light output unit 612 emits an optical signal PL, which is an ultrashort pulsed light that has been pulse-amplitude modulated. The optical signal PL emitted from the light output unit 612 is focused into the antiferromagnetic layer 620 by the lens 614. Here, since the optical signal PL is pulsed light, the magnetic order of the antiferromagnetic layer 620 is reversed when light with an intensity equal to or greater than a threshold is irradiated, but the magnetic order is not reversed when light with an intensity below the threshold is irradiated. In this manner, data corresponding to the optical signal PL can be written to the antiferromagnetic layer 620. When reading data stored in the antiferromagnetic layer 620, the anomalous Hall effect can be used, for example, as in Examples 1 and 4 (FIGS. 7 and 10).

[0079] Unlike Examples 4 and 5 (FIGS. 10 and 11), the photonic spin register 600 does not require a photodetector (i.e., there is no need to convert the optical signal PL into a photocurrent), and can directly control the direction of the magnetic order in the antiferromagnetic layer 620 with light. Therefore, power consumption due to photocurrent can be completely suppressed.

[0080] In addition, in Example 1 (FIG. 7), a magnetic memory device including a plurality of magnetic memory elements 100 may be configured. Also, in Example 2 (FIG. 8), a magnetic memory device may be configured in which a plurality of magnetic memory elements 200 are arranged in a matrix. Similarly, in Example 3 (FIG. 9), a magnetic memory device may be configured in which a plurality of magnetic memory elements 300 are arranged in a matrix. Furthermore, a computer system or an information processing system may be configured that includes the magnetic memory elements of Examples 1 to 3 or the photonic spin registers of Examples 4 to 6.

[0081] In Examples 1 and 2 (FIGS. 7 and 8) and Examples 4 and 5 (FIGS. 10 and 11), a spin Hall layer was placed in contact with the antiferromagnetic layer (free layer) and the magnetic order of the antiferromagnetic layer was reversed by SOT. However, in these Examples, magnetic order reversal can be expected even with a single antiferromagnetic layer without the spin Hall layer.

[0082] The present invention is not limited to the above-described embodiment, and various modifications are possible within the scope of the present invention.

[0083] 1, 10 Substrate 2, 14, 440, 620 Antiferromagnetic layer 12, 220, 430, 530 Spin Hall layer 100, 200, 300, 420, 520 Magnetic memory element 210, 310, 540 Magnetoresistance element 212, 312 Free layer 214, 314 Nonmagnetic layer 216, 316 Reference layer 400, 500, 600 Photonic spin register 410 Optical receiver 412 Optical waveguide 414 Photodetector 416 Photoelectric conversion element 610 Light irradiation unit

Claims

1. A magnetic memory element comprising a polycrystalline antiferromagnetic layer made of an antiferromagnetic material exhibiting an anomalous Hall effect, having one or more first grains with an average grain size in the range of 20 nm to 200 nm, and having a plurality of second grains within each first grain, wherein the magnetic order of the antiferromagnetic material is reversible.

2. The magnetic memory element according to claim 1, wherein the average grain size of each of the second grains is equal to or less than half the average grain size of each of the first grains.

3. The magnetic memory element according to claim 2, wherein the average grain size of each of the second grains is in the range of 1 / 20 to 1 / 2 of the average grain size of each of the first grains.

4. The magnetic memory element according to claim 1, wherein the antiferromagnetic body has a spin structure that macroscopically breaks time-reversal symmetry.

5. The magnetic memory element of claim 1, wherein said antiferromagnetic material is a canted antiferromagnetic material.

6. The magnetic memory element of claim 1, wherein said antiferromagnetic body has a spin order of cluster magnetic octopoles.

7. A magnetic memory element according to any one of claims 1 to 6, comprising a spin Hall layer in contact with the antiferromagnetic layer, made of a material exhibiting the spin Hall effect, in which a spin current is generated in a direction perpendicular to the plane when a write current flows in an in-plane direction, wherein in the antiferromagnetic layer, a spin orbit torque generated by the spin current acts on the magnetic order of the antiferromagnetic material, thereby enabling the magnetic order to be reversed.

8. A magnetic memory element according to any one of claims 1 to 6, comprising: a spin Hall layer made of a material exhibiting the spin Hall effect, in which a spin current is generated in a direction perpendicular to the plane when a write current flows in an in-plane direction; a free layer in contact with the spin Hall layer, which is an antiferromagnetic layer and in which the magnetic order of the antiferromagnetic material can be reversed when a spin-orbit torque generated by the spin current acts on the magnetic order of the antiferromagnetic material; a reference layer made of a magnetic material in which the magnetic order of the magnetic material is fixed; and a non-magnetic layer provided between the free layer and the reference layer.

9. A magnetic memory element according to any one of claims 1 to 6, comprising: a reference layer made of a magnetic material in which the magnetic order of the magnetic material is fixed; a free layer which is an antiferromagnetic layer in which the magnetic order of the antiferromagnetic material can be reversed by spin transfer torque when a write current flows in the perpendicular direction; and a non-magnetic layer provided between the reference layer and the free layer.

10. A magnetic memory device comprising a plurality of magnetic memory elements, each of the plurality of magnetic memory elements being defined as a magnetic memory element according to claim 7.

11. A magnetic memory device comprising a plurality of magnetic memory elements, each of the plurality of magnetic memory elements being defined as a magnetic memory element according to claim 8.

12. A magnetic memory device comprising a plurality of magnetic memory elements, each of the plurality of magnetic memory elements being defined as a magnetic memory element according to claim 9.

13. A photonic spin register comprising: a magnetic memory element as defined in claim 7; and a photoreceiver for receiving a pulse amplitude modulated optical signal and converting it into a photocurrent, wherein when the photocurrent flows in the in-plane direction as the write current in the spin Hall layer, a spin current is generated in the perpendicular direction to the plane.

14. A photonic spin register comprising: a magnetic memory element as defined in claim 8; and a photoreceiver for receiving a pulse amplitude modulated optical signal and converting it into a photocurrent, wherein when the photocurrent flows in the in-plane direction as the write current in the spin Hall layer, a spin current is generated in the perpendicular direction to the plane.

15. A photonic spin register comprising: a magnetic memory element according to any one of claims 1 to 6; and a light irradiation unit which irradiates the antiferromagnetic layer with a pulse amplitude modulated optical signal, wherein the magnetic order of the antiferromagnetic material in the antiferromagnetic layer can be reversed by irradiation with the optical signal.

Citation Information

Patent Citations

  • Exchange coupled film and magneto-resistance effect device using the same, magnetic head and magnetic storage device

    JP1998284321A

  • Spintronics element and magnetic memory device

    WO2020166722A1

  • Photonic spin register, information writing method, and information read-out method

    WO2022158545A1

  • Magnetic memory element

    WO2022220251A1