Spunbonded nonwoven fabric, tape, and method for producing spunbonded nonwoven fabric

The spunbond nonwoven fabric, made with polyethylene terephthalate resin and a core-sheath composite structure, addresses the trade-off between mechanical strength and hand-tearability, offering a balanced solution for tape applications with enhanced properties.

WO2024204333A1PCT designated stage expired Publication Date: 2024-10-03TORAY INDUSTRIES INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012232
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional spunbond nonwoven fabric tapes face a trade-off between mechanical strength and hand-tearability, with increased crimping for better hand-tearability leading to reduced adhesion and mechanical strength, and nonwoven fabrics with high tear strength having poor hand-tearability.

Method used

A spunbond nonwoven fabric composed of polyethylene terephthalate resin fibers with specific crystallization and melting peak ranges, core-sheath composite structure, and controlled thermocompression bonding, resulting in a fabric with enhanced mechanical strength and hand-tearability.

Benefits of technology

The solution provides a nonwoven fabric with balanced mechanical strength and hand-tearability, suitable for practical applications, including building and medical uses, by optimizing fiber composition and processing techniques.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012232_03102024_PF_FP_ABST
    Figure JP2024012232_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing a nonwoven fabric having excellent mechanical strength and excellent hand tearability. The present invention is a spunbonded nonwoven fabric composed of fibers each containing a polyethylene terephthalate-based resin as a main component, wherein a crystallization peak appears in a range of 100°C to 150°C and a single melting peak appears in a range of 250°C to 270°C according to differential scanning calorimetry, and the fabric has an emboss compression rate of 5% by area to 30% by area.
Need to check novelty before this filing date? Find Prior Art

Description

Spunbond nonwoven fabric, tape, and method for producing spunbond nonwoven fabric

[0001] The present invention relates to spunbond nonwoven fabrics and tapes.

[0002] Adhesive tapes are used in a variety of fields, including building materials, vehicles, and medical applications, and tape substrates include paper, cloth, nonwoven fabric, and film. In particular, paper is often used as the tape substrate in fields where hand-tearability, i.e., the ability of a tape to be easily torn by hand by a worker when in use, is required. However, because paper-based tapes can sometimes lack strength, nonwoven fabrics are sometimes used instead. However, when nonwoven fabrics are used, the high tear strength and poor hand-tearability pose a challenge.

[0003] Patent Document 1 proposes a nonwoven fabric tape substrate characterized by being made of a synthetic long fiber nonwoven fabric having a fiber diameter, apparent density, basis weight, and partial thermocompression bonding rate within specific ranges, a longitudinal tensile strength and breaking elongation of at least a certain level, and linear or broken line-shaped thermocompression-bonded portions that are different from the thermocompression-bonded portions and are perpendicular to the longitudinal direction.

[0004] JP 2012-180615 A

[0005] In the nonwoven fabric disclosed in Patent Document 1, linear or dashed line-shaped compression sections added after thermocompression bonding can reduce tear strength and improve hand-tearability. However, in the nonwoven fabric subjected to the above-mentioned compression processing, as the number of compression sections increases, the surface becomes more uneven, which deteriorates adhesion to the installation surface when used as a tape substrate. Furthermore, in order to improve hand-tearability by increasing the number of compression sections, it is necessary to compress the nonwoven fabric until it becomes a film. As the number of film-like sections increases, the mechanical strength (tensile strength) of the nonwoven fabric decreases, so it cannot be said that it is sufficient to achieve both mechanical strength and hand-tearability.

[0006] SUMMARY OF THE INVENTION It is therefore an object of the present invention to provide a nonwoven fabric and, in turn, a tape that has excellent mechanical strength and is easy to tear by hand.

[0007] As a result of extensive research aimed at achieving the above object, the present inventors have discovered that by adjusting the crystallization peak and melting peak of a spunbonded nonwoven fabric in a specific temperature range as measured by differential scanning calorimetry, a spunbonded nonwoven fabric having excellent mechanical strength and excellent hand-tearability can be obtained. The present invention was completed based on this discovery.

[0008] The present invention and its preferred embodiments include the following configurations.

[0009] [1] A spunbond nonwoven fabric composed of fibers containing polyethylene terephthalate resin as a main component, which has a crystallization peak in the range of 100°C to 150°C and a single melting peak in the range of 250°C to 270°C, measured by differential scanning calorimetry, and has an embossing rate of 5 area % to 30 area %.

[0010] [2] The nonwoven fabric according to the above [1], wherein the fiber breakage rate per unit area in the non-pressed portion is 5.0% or more and 50.0% or less.

[0011] [3] A tape comprising the spunbond nonwoven fabric according to [1] or [2]. [4] A method for producing the spunbond nonwoven fabric according to [1] or [2], comprising the following steps (a) to (c) in this order: Step (a): Spinning a core-sheath composite fiber comprising a high-viscosity polyethylene terephthalate resin having a melting point of 250°C or higher and 270°C or lower, surrounded by a low-viscosity polyethylene terephthalate resin having a melting point of 250°C or higher and 270°C or lower, the low-viscosity polyethylene terephthalate resin having an intrinsic viscosity (IV) lower than that of the high-viscosity polyethylene terephthalate resin by 0.05 to 0.25. Step (b): Pulling and stretching the spun core-sheath composite fiber with an ejector and depositing it on a moving net conveyor to form a fiber web. Step (c): Thermocompressing the fiber web to an embossing ratio of 5 to 30 area %.

[0012] According to the present invention, a nonwoven fabric having excellent mechanical strength and easy hand tearing is provided.

[0013] FIG. 1 is a scanning electron micrograph of a non-bonded portion containing rotten fibers in a spunbond nonwoven fabric of the present invention.

[0014] The spunbond nonwoven fabric of the present invention is a spunbond nonwoven fabric composed of fibers containing polyethylene terephthalate resin as a main component, and has a crystallization peak in the range of 100°C to 150°C and a single melting peak in the range of 250°C to 270°C as measured by differential scanning calorimetry, and an embossing rate of 5% to 30% by area. The components thereof will be described in detail below, but the present invention is not limited to the scope described below as long as it does not deviate from the gist of the invention, and various modifications are possible within the scope of the invention.

[0015] [Polyethylene terephthalate resin] First, the spunbond nonwoven fabric of the present invention is composed of fibers containing polyethylene terephthalate resin as a main component.

[0016] The melting point of the polyethylene terephthalate resin is preferably 250°C or higher and 270°C or lower. By setting the melting point of the polyethylene terephthalate resin to 250°C or higher, heat resistance sufficient for practical use is easily obtained. Furthermore, by setting the melting point of the polyethylene terephthalate resin to 270°C or lower, it becomes easier to cool the yarn discharged from the spinneret, suppressing fusion of fibers and facilitating stable spinning even with a fine fiber diameter. Here, the melting point of the polyethylene terephthalate resin refers to the maximum melting peak temperature obtained by measuring the polyethylene terephthalate resin by differential scanning calorimetry (DSC).

[0017] The intrinsic viscosity (IV) of the polyethylene terephthalate resin is preferably 0.40 or more and 0.70 or less. By making the intrinsic viscosity of the polyethylene terephthalate resin 0.40 or more, more preferably 0.45 or more, and even more preferably 0.50 or more, it is possible to suppress a decrease in the strength of the fibers constituting the nonwoven fabric. On the other hand, by making the intrinsic viscosity of the polyethylene terephthalate resin 0.70 or less, it is possible to stably spin even fine fibers, and to obtain a spunbond nonwoven fabric having a uniform texture and sufficient strength for practical use.

[0018] To the polyethylene terephthalate resin, additives such as a crystal nucleating agent, a matting agent, a lubricant, a pigment, an antifungal agent, an antibacterial agent, a flame retardant, a metal oxide, an aliphatic bisamide and / or an alkyl-substituted aliphatic monoamide, and a hydrophilic agent can be added within a range that does not impair the effects of the present invention. Among these, metal oxides such as titanium oxide have the effect of reducing the surface friction of the fibers and preventing fusion of the fibers to improve spinnability, and also improving the fusion properties of the nonwoven fabric by increasing thermal conductivity during fusion molding of the nonwoven fabric with a heated roll, thereby making it possible to obtain a spunbond nonwoven fabric with superior mechanical strength.

[0019] [Fibers] The fibers constituting the nonwoven fabric are preferably core-sheath type composite fibers.

[0020] Furthermore, the intrinsic viscosity (IV) of the polyethylene terephthalate resin of the sheath component is preferably lower than the intrinsic viscosity (IV) of the polyethylene terephthalate resin of the core component by a range of 0.05 to 0.25. Hereinafter, the polyethylene terephthalate resin of the sheath component in this embodiment will also be referred to as the "low-viscosity polyethylene terephthalate resin," and the polyethylene terephthalate resin of the core component will also be referred to as the "high-viscosity polyethylene terephthalate resin." When the intrinsic viscosity of the low-viscosity polyethylene terephthalate resin is lower than the intrinsic viscosity of the high-viscosity polyethylene terephthalate resin by 0.05 or more, more preferably 0.08 or more, and even more preferably 0.10 or more, spinning stress is concentrated on the core component during spinning, promoting the orientation of the core component and suppressing the orientation of the sheath component. As a result, a fiber with high single fiber strength and excellent thermal adhesiveness can be obtained, making it easier to obtain a nonwoven fabric with excellent mechanical strength. On the other hand, when the intrinsic viscosity of the low-viscosity polyethylene terephthalate resin is lower than the intrinsic viscosity of the high-viscosity polyethylene terephthalate resin by 0.25 or less, preferably 0.20 or less, the single fiber strength of the sheath-core composite fiber can be improved.

[0021] The intrinsic viscosity (IV) of the high-viscosity polyethylene terephthalate resin is preferably 0.55 or more and 0.70 or less. By making the intrinsic viscosity of the high-viscosity polyethylene terephthalate resin 0.55 or more, a decrease in single fiber strength can be prevented. Furthermore, by making the intrinsic viscosity of the high-viscosity polyethylene terephthalate resin 0.70 or less, it is possible to stably spin even fine fibers, and to obtain a spunbond nonwoven fabric having a uniform texture and sufficient strength for practical use.

[0022] The mass ratio of the sheath component in the sheath-core composite fiber is preferably 10% by mass or more and 80% by mass or less. When the mass ratio of the sheath component is 10% by mass or more, more preferably 15% by mass or more, and even more preferably 20% by mass or more, the sheath components are firmly fused together during thermal bonding, resulting in a spunbonded nonwoven fabric having sufficient strength for practical use. On the other hand, when the mass ratio of the sheath component is 80% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less, the proportion of the highly oriented core component is increased, improving the single fiber strength of the sheath-core composite fiber, resulting in a spunbonded nonwoven fabric having sufficient strength for practical use.

[0023] The composite form of the sheath-core composite fiber may be, for example, a concentric sheath-core type, an eccentric sheath-core type, an islands-in-sea type, etc. Among these, the sheath-core type composite form is preferred, and the concentric sheath-core type composite form is more preferred, because it has excellent spinnability and can be used to form a spunbonded nonwoven fabric with excellent mechanical strength by uniformly bonding the fibers together through thermal bonding.

[0024] The fibers preferably have an average single fiber diameter of 6.0 μm or more and 20.0 μm or less. By making the average single fiber diameter 6.0 μm or more, more preferably 7.0 μm or more, and even more preferably 8.0 μm or more, it is possible to prevent a decrease in spinnability, improve production stability, and obtain a spunbond nonwoven fabric having excellent mechanical strength. On the other hand, by making the average single fiber diameter 20.0 μm or less, more preferably 18.0 μm or less, and even more preferably 16.0 μm or less, it is possible to obtain a spunbond nonwoven fabric having a uniform texture and sufficient strength for practical use.

[0025] In the present invention, the average single fiber diameter (μm) is determined by the following method. (i) Ten small sample pieces measuring 10 mm x 10 mm are randomly collected from a spunbond nonwoven fabric. (ii) The surfaces of the collected small sample pieces are photographed using a scanning electron microscope or the like at a magnification of 500 to 2000 times, allowing the fiber thickness to be measured. (iii) Ten fibers are randomly selected from the photographs of each small sample piece, for a total of 100 fibers, and their thicknesses are measured. The fibers are assumed to have a circular cross section, and the thickness is taken as the fiber diameter. (iv) The arithmetic mean value of these values ​​is rounded to one decimal place, and the calculated value is taken as the average single fiber diameter.

[0026] [Spunbonded Nonwoven Fabric] The spunbonded nonwoven fabric of the present invention has a crystallization peak in the range of 100°C or higher and 150°C or lower, as measured by differential scanning calorimetry. Having a crystallization peak temperature within this range promotes fusion between fibers during embossing and compression, resulting in a spunbonded nonwoven fabric with excellent tensile strength. Furthermore, since the fibers in the non-bonded portions are torn by heat, the spunbonded nonwoven fabric has low tear strength and excellent hand-tearability. On the other hand, in the case of a spunbonded nonwoven fabric that does not have a crystallization peak, not only is fusion between fibers less likely to occur, resulting in a nonwoven fabric with low tensile strength, but also, since the fibers in the non-bonded portions are not torn, the fibers are difficult to tear, resulting in a spunbonded nonwoven fabric with poor hand-tearability.

[0027] Furthermore, the spunbond nonwoven fabric has a single melting peak in the range of 250° C. to 270° C. as measured by differential scanning calorimetry. By having a single melting peak in this range, the fibers can be firmly thermally bonded together at a sufficient temperature without causing operational problems such as the low-melting point component melting and sticking to the heated roll during thermal bonding, and a spunbond nonwoven fabric having sufficient strength for practical use can be obtained.

[0028] Here, the crystallization peak temperature Tc (°C) and melting peak temperature Tm (°C) of the spunbond nonwoven fabric are obtained by differential scanning calorimetry (DSC), and values ​​calculated by the following procedure are adopted: (1) A small piece of spunbond nonwoven fabric is sampled in an amount of 0.5 to 5 mg. (2) Using differential scanning calorimetry (DSC), the temperature is raised from room temperature to 280°C at a heating rate of 16°C / min to obtain a DSC curve. (3) From the DSC curve, the peak-top temperature of the crystallization exothermic peak is read and designated as the crystallization peak temperature Tc (°C) of the spunbond nonwoven fabric, and the peak-top temperature of the melting endothermic peak is read and designated as the melting peak temperature Tm (°C) of the spunbond nonwoven fabric.

[0029] The spunbonded nonwoven fabric has an embossing rate of 5 area% or more and 30 area% or less. By setting the embossing rate to 5 area% or more, more preferably 8 area% or more, and even more preferably 10 area% or more, it is possible to obtain a strength sufficient for practical use as a spunbonded nonwoven fabric. On the other hand, by setting the embossing rate to 30 area% or less, more preferably 25 area% or less, and even more preferably 20 area% or less, it is possible to reduce the unevenness of the nonwoven fabric surface and obtain sufficient adhesion when used as a tape.

[0030] The embossing rate here refers to the proportion of the area of ​​the bonded portion to the total area of ​​the spunbonded nonwoven fabric. Specifically, when thermocompression bonding is performed using a pair of uneven rolls, it refers to the proportion of the area of ​​the portion of the spunbonded nonwoven fabric where the convex portions of the upper roll and the convex portions of the lower roll overlap and contact the fibrous web (bonded portion). When thermocompression bonding is performed using an uneven roll and a flat roll, it refers to the proportion of the area of ​​the portion of the uneven roll where the convex portions of the uneven roll contact the fibrous web (bonded portion) to the total area of ​​the spunbonded nonwoven fabric.

[0031] The spunbonded nonwoven fabric preferably has a fiber fray rate per unit area in the non-bonded portions of 5.0% or more and 50.0% or less. A fiber fray rate of 5.0% or more, more preferably 7.0% or more, and even more preferably 10.0% or more reduces tear strength and provides sufficient hand tearability for practical use as a tape substrate. On the other hand, a fiber fray rate of 50.0% or less, more preferably 40.0% or less, and even more preferably 30.0% or less, can suppress excessive fiber fraying and prevent a decrease in tensile strength. In the present invention, the fiber fray rate refers to a value measured and calculated by the following method. (i) Ten small sample pieces each for observation of the front surface and the back surface of the nonwoven fabric are taken (20 pieces in total). (ii) The collected small sample is subjected to scanning electron microscopy (SEM, for example, Keyence Corporation's "VHX-D500") at a magnification of 2000 times to measure an area of ​​22000 μm. 2 (iii) In the photographs of each small sample, the total number of fibers (N) and the number of fibers (n) with frayed portions (3) of 10 μm or more in the length direction of the fibers as shown in FIG. 1 are counted, and the fiber fray rate is calculated using the following formula: Fiber fray rate (%) = (n / N) x 100 (iv) The arithmetic mean values ​​of 10 small sample pieces on each of the front and back surfaces are calculated and rounded to one decimal place. The fray rates on the front and back surfaces are compared, and the larger value is taken as the fiber fray rate of the spunbond nonwoven fabric.

[0032] The spunbond nonwoven fabric of the present invention has a tensile strength per unit area of ​​5.00 (N / 5cm) / (g / m 2 It is preferable that the tensile strength is 5.00 (N / 5cm) / (g / m 2 ) or more, more preferably 5.50 (N / 5cm) / (g / m 2 ) or more, more preferably 5.80 (N / 5cm) / (g / m 2 ) or more, the minimum tensile strength required for a tape substrate can be achieved, which is preferable from the viewpoint of tape processability.

[0033] In the present invention, the tensile strength per unit area of ​​the spunbonded nonwoven fabric ((N / 5 cm) / (g / m 2)) shall be the value determined by the following method in accordance with 6.3 "Tensile Strength and Elongation" of JIS L1913:2010 "Test Methods for General Long-Fiber Nonwoven Fabrics." (i) Three samples of 30 cm x 5.0 cm width shall be taken from the nonwoven fabric at equal intervals in both the MD and CD directions. (ii) A load shall be applied until the sample breaks under conditions of a gripping distance of 20 cm and a pulling speed of 100±10 mm / min. (iii) The strength of the sample at the maximum load shall be taken as the tensile strength (N / 5 cm), and the average values ​​of three points in each of the MD and CD directions shall be calculated. The sum of these average values ​​shall be taken as the tensile strength of the spunbond nonwoven fabric. (iv) The tensile strength per unit area of ​​the spunbond nonwoven fabric ((N / 5 cm) / (g / m)) shall be calculated based on the following formula: 2 )) is calculated and rounded to two decimal places. 2 )) = [tensile strength of spunbond nonwoven fabric (N / 5 cm)] / basis weight (g / m 2 ).

[0034] The spunbond nonwoven fabric of the present invention has a tear strength per unit area of ​​0.10 N / (g / m 2 ) or more 1.00N / (g / m 2 It is preferable that the tear strength is 0.10 N / (g / m) or less. 2 ) or more, more preferably 0.15 N / (g / m 2 ) or more, the minimum tear strength required for a tape substrate can be achieved, which is preferable from the viewpoint of tape processability. 2 ) or less, more preferably 0.90 N / (g / m 2 ) or less, more preferably 0.80 N / (g / m 2 ) or less, the hand tearability after tape processing can be more effectively improved.

[0035] In the present invention, the tear strength per unit area weight of a spunbond nonwoven fabric is measured using a constant-rate extension tensile tester (e.g., Baldwin's "RTG-1250") in accordance with JIS L1913:2010 "Testing Methods for General Nonwoven Fabrics," section 6.4 "Tear Strength," a) Trapezoid Method, as follows: (i) Three 25 cm x 5.0 cm wide samples are taken from the nonwoven fabric, each equally spaced in the MD direction. (ii) An isosceles trapezoid mark is made on the test piece, and a 1.0 cm incision is made at a right angle to the short side at the center of the short side of the mark. (iii) The test piece is attached to the grips of the constant-rate extension tensile tester along the mark, with the short side of the trapezoid tensile tensioned and the long side relaxed, with a grip distance of 10 cm. (iv) The maximum load when torn under the condition of a pulling speed of 100±10 mm / min is taken as the tear strength (N), and the average value of three points is calculated to be the tear strength (N) of the spunbond nonwoven fabric. (v) The tear strength per unit area of ​​the spunbond nonwoven fabric (N / (g / m)) is calculated based on the following formula. 2 )) is calculated and rounded to two decimal places. 2 )) = [Tear strength of spunbond nonwoven fabric (N)] / basis weight (g / m 2 ).

[0036] [Method for producing spunbonded nonwoven fabric] The spunbonded nonwoven fabric of the present invention can be preferably produced by the method for producing spunbonded nonwoven fabric of the present invention. That is, the method for producing spunbonded nonwoven fabric of the present invention is a method for producing the spunbonded nonwoven fabric of the present invention, and includes the following steps (a) to (c) in this order:

[0037] [Step (a): Step of Spinning Fibers] In step (a), a core-sheath type composite fiber is spun, in which a low-viscosity polyethylene terephthalate resin having a melting point of 250°C or higher and 270°C or lower, and having an intrinsic viscosity (IV) that is 0.05 or higher and 0.25 or lower than the intrinsic viscosity (IV) of the high-viscosity polyethylene terephthalate resin, is disposed around the high-viscosity polyethylene terephthalate resin having a melting point of 250°C or higher and 270°C or lower.

[0038] That is, in the sheath-core composite fiber, it is preferable that the high-viscosity polyethylene terephthalate resin be the core component and the low-viscosity polyethylene terephthalate resin be the sheath component. By making the difference between the intrinsic viscosities of the core component and the sheath component 0.05 or more, more preferably 0.10 or more, spinning stress can be concentrated on the core component during spinning, promoting the orientation of the core component and suppressing the orientation of the sheath component. On the other hand, by making the difference between the intrinsic viscosities of the core component and the sheath component 0.25 or less, preferably 0.20 or less, the strength of the single fiber of the sheath-core composite fiber can be improved, and rapid softening during thermal bonding can be suppressed, thereby suppressing sticking to heated rolls during production.

[0039] The core-sheath type composite fiber is preferably melted at a temperature of not less than its melting point but not more than 70°C above the melting point, and melt-extruded from a spinneret at a temperature of not less than its melting point but not more than 70°C above the melting point.

[0040] The shape of the outlet hole of the spinneret through which the core-sheath type composite fiber is extruded can be circular, elliptical, polygonal, multi-lobal, or a combination thereof, depending on the cross-sectional shape of the fiber. Among these, a circular shape is more preferred from the viewpoints of efficiently obtaining bonding points between the fibers and firmly bonding the fibers together by thermocompression bonding.

[0041] [Step (b): Step of forming a fiber web] In step (b), the spun core-sheath type composite fibers are pulled and stretched by an ejector and deposited on a moving net conveyor to form a fiber web.

[0042] In step (b), the spun fibers are preferably drawn and stretched by an ejector, and the fibers are deposited on a moving net conveyor to form a fiber web. In this case, the spinning speed for drawing the fibers is preferably 3000 m / min or more and 6000 m / min or less.

[0043] [Step (c): Step of thermocompression bonding of fiber web] In step (c), the fiber web is thermocompression bonded to an embossing rate in the range of 5 area % to 30 area %.

[0044] The fiber web can be heat-pressed to obtain the intended spunbonded nonwoven fabric.

[0045] Examples of methods for thermocompression bonding the fiber web include methods of thermocompression bonding using various rolls, such as a heat embossing roll having an engraving (uneven portion) on the surface of a pair of upper and lower rolls, and a heat embossing roll consisting of a combination of a roll with one flat (smooth) surface and a roll with an engraving (uneven portion) on the surface of the other roll. Among these, it is preferable to use a heat embossing roll having an engraving (uneven portion) on the surface of a pair of upper and lower rolls, or a heat embossing roll consisting of a combination of a roll with one flat (smooth) surface and a roll with an engraving (uneven portion) on the surface of the other roll, because these methods are highly productive and can impart strength to the partially thermocompression-bonded parts while maintaining the texture unique to nonwoven fabrics in the non-bonded parts.

[0046] As for the surface material of the hot embossing roll, a preferred embodiment is to use a pair of metal rolls in order to obtain a sufficient thermocompression effect and to prevent the engraving (concave and convex portions) of one embossing roll from being transferred to the surface of the other roll.

[0047] The embossing rate by the hot embossing roll is 5 area % or more and 30 area % or less. By setting the embossing rate to 5 area % or more, preferably 8 area % or more, and more preferably 10 area % or more, it is possible to obtain a strength sufficient for practical use as a spunbond nonwoven fabric. On the other hand, by setting the embossing rate to 30 area % or less, preferably 25 area % or less, and more preferably 20 area % or less, it is possible to reduce the unevenness of the nonwoven fabric surface and obtain sufficient adhesion when used as a tape.

[0048] The shape of the part pressed by the heat embossing roll may be, for example, a circle, an oval, a square, a rectangle, a parallelogram, a rhombus, a regular hexagon, or a regular octagon.

[0049] It is also preferable that the compressed portions are uniformly spaced at regular intervals in both the longitudinal direction (machine direction) and the width direction of the spunbonded nonwoven fabric, thereby reducing variations in strength of the spunbonded nonwoven fabric.

[0050] The surface temperature of the hot embossing roll during thermocompression bonding is preferably 10°C to 100°C lower than the melting point (hereinafter sometimes referred to as Tm (°C)) of the polyethylene terephthalate resin being used (i.e., (Tm - 100)°C to (Tm - 10)°C). By setting the surface temperature of the hot roll to (Tm - 100)°C or higher, more preferably (Tm - 90)°C or higher, it is possible to obtain a spunbonded nonwoven fabric with adequate thermocompression bonding strength for practical use. Furthermore, by setting the surface temperature of the hot embossing roll to (Tm - 10)°C or lower, more preferably (Tm - 15)°C or lower, excessive thermocompression bonding can be suppressed, and the spunbonded nonwoven fabric can be prevented from partially forming a film-like sheet.

[0051] The linear pressure of the hot embossing roll during thermocompression bonding is preferably 90 N / cm or more and 1000 N / cm or less. By setting the linear pressure for thermocompression bonding to 90 N / cm or more, a spunbond nonwoven fabric with excellent mechanical strength can be obtained. By setting the linear pressure for thermocompression bonding to 1000 N / cm or less, excessive fusion between fibers can be prevented.

[0052] [Tape] The tape of the present invention includes the nonwoven fabric. This allows for a tape with excellent mechanical strength and easy hand tearing. The tape referred to here refers to a tape having an adhesive layer on at least one side of a nonwoven fabric substrate and a width of 150 mm or less.

[0053] The tape of the present invention can be used in various fields, such as construction material applications, vehicle applications, and medical applications. In particular, it is suitable for construction material applications that require hand tearability. Specific examples of the tape of the present invention include adhesive tape, curing tape, masking tape, and sealing tape.

[0054] Next, the nonwoven fabric of the present invention will be specifically described based on examples, although the present invention is not limited to these examples.

[0055] [Measurement Methods] The evaluation methods and measurement conditions used in the examples are described below. Unless otherwise specified, the measurements of each physical property were carried out according to the above-mentioned methods.

[0056] (1) Melting Point (°C) of Polyethylene Terephthalate Resin Using a differential scanning calorimeter ("DSC-2" manufactured by PerkinElmer Co., Ltd.), measurement was performed at a temperature rise rate of 16°C / min, and the temperature at which the extreme value was obtained in the obtained melting endothermic curve was taken as the melting point.

[0057] (2) Intrinsic Viscosity (IV) of Polyethylene Terephthalate Resin The intrinsic viscosity (IV) of the polyethylene terephthalate resin was measured by the following method.

[0058] 8 g of sample was dissolved in 100 mL of orthochlorophenol, and the relative viscosity η was measured at 25°C using an Ostwald viscometer. r was calculated using the following formula: η r = η / η 0 = (t × d) / (t 0 ×d 0 ) where η is the viscosity of the polymer solution, η 0 is the viscosity of orthochlorophenol, t is the solution drop time (seconds), and d is the solution density (g / cm 3 ), t 0 is the fall time of orthochlorophenol (seconds), d 0 is the density of orthochlorophenol (g / cm 3 ) respectively. Next, the relative viscosity η r The intrinsic viscosity (IV) was calculated from the following formula: Intrinsic viscosity (IV) = 0.0242η r +0.2634.

[0059] (3) Average Single Fiber Diameter (μm) of Fibers The average single fiber diameter of fibers was calculated by the above-mentioned method using a scanning electron microscope "VHX-D500" manufactured by Keyence Corporation.

[0060] (4) Crystallization Peak Temperature (Tc) of Spunbond Nonwoven Fabric The crystallization peak temperature of the spunbond nonwoven fabric was calculated by the above-mentioned method using a differential scanning calorimeter, "DSC-2 Model" manufactured by PerkinElmer Co., Ltd.

[0061] (5) Melting Peak Temperature (Tm) of Spunbond Nonwoven Fabric The melting peak temperature of the spunbond nonwoven fabric was calculated by the above-mentioned method using a differential scanning calorimeter "DSC-2 Model" manufactured by PerkinElmer Co., Ltd.

[0062] (6) Fiber Torn Rate (%) The fiber torn rate in the spunbond nonwoven fabric was calculated by the above-mentioned method using a scanning electron microscope "VHX-D500" manufactured by Keyence Corporation.

[0063] (7) Tensile strength per unit area of ​​spunbond nonwoven fabric ((N / 5cm) / (g / m 2 ) The tensile strength per unit area of ​​the spunbond nonwoven fabric was measured by the above-mentioned method using a constant-speed extension tensile tester "RTG-1250" manufactured by Baldwin.

[0064] (8) Tear strength per unit area of ​​spunbond nonwoven fabric (N / (g / m 2 ) The tear strength per unit area of ​​the spunbond nonwoven fabric was measured by the above-mentioned method using a constant-speed extension tensile tester "RTG-1250" manufactured by Baldwin.

[0065] [Resins Used] Details of the resins used in the Examples and Comparative Examples are described below. Polyethylene terephthalate resin A (PET_A): polyethylene terephthalate dried to a moisture content of 50 mass ppm or less, having an intrinsic viscosity (IV) of 0.65 and a melting point of 255°C. Polyethylene terephthalate resin B (PET_B): polyethylene terephthalate dried to a moisture content of 50 mass ppm or less, having an intrinsic viscosity (IV) of 0.51 and a melting point of 255°C. Polyethylene terephthalate resin C (PET_C): polyethylene terephthalate dried to a moisture content of 50 mass ppm or less, having an intrinsic viscosity (IV) of 0.70 and a melting point of 255°C. Polyethylene terephthalate resin D (PET_D): polyethylene terephthalate dried to a moisture content of 50 mass ppm or less, having an intrinsic viscosity (IV) of 0.56 and a melting point of 255°C. Polyethylene terephthalate resin E (PET_E): Polyethylene terephthalate dried to a moisture content of 50 mass ppm or less, having an intrinsic viscosity (IV) of 0.45 and a melting point of 255°C. Polyethylene terephthalate resin F (PET_F): Polyethylene terephthalate dried to a moisture content of 50 mass ppm or less, having an intrinsic viscosity (IV) of 0.62 and a melting point of 255°C. Polyethylene terephthalate resin G (CO-PET): Copolymerized polyethylene terephthalate dried to a moisture content of 50 mass ppm or less, having an intrinsic viscosity (IV) of 0.64, an isophthalic acid copolymerization rate of 11 mol%, and a melting point of 230°C.

[0066] [Example 1] (Step of spinning fibers) Polyethylene terephthalate resin A and polyethylene terephthalate resin B were each melted at a temperature of 295° C. Next, concentric sheath-core composite fibers were spun from a circular nozzle using polyethylene terephthalate resin A as a core component and polyethylene terephthalate resin B as a sheath component at a spinneret temperature of 295° C. and a core:sheath mass ratio of 80:20.

[0067] (Step of forming a fiber web) The fibers spun in the above step were drawn at a spinning speed of 5000 m / min, and the basis weight of the resulting nonwoven fabric was 80.0 g / m 2The mixture was deposited on a net conveyor whose moving speed was adjusted so that the diameter of the fibers was 12.1 μm, thereby forming a fiber web made of fibers having a fiber diameter of 12.1 μm.

[0068] (Step of thermocompression bonding of fiber web) Subsequently, the formed fiber web was thermocompression bonded using a pair of upper and lower thermal embossing rolls consisting of an upper roll and a lower roll under the conditions of a surface temperature of the thermal embossing roll of 170°C and a linear pressure of 686 N / cm to obtain a spunbonded nonwoven fabric. Upper roll: a metallic embossing roll with a bonding area ratio of 16%. Lower roll: a metallic flat roll.

[0069] The spunbonded nonwoven fabric obtained was evaluated, and the results are shown in Table 1.

[0070] [Example 2] In the step of thermocompression bonding the fiber web, an embossing roll with a bonded area ratio of 8% was used as the upper roll. Except for this, a spunbonded nonwoven fabric was obtained using the same procedure and conditions as in Example 1. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.

[0071] [Example 3] In the step of thermocompression bonding the fiber web, an embossing roll with a bonding area ratio of 20% was used as the upper roll. Except for this, a spunbonded nonwoven fabric was obtained using the same procedure and conditions as in Example 1. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.

[0072] [Example 4] In the fiber spinning process, polyethylene terephthalate resin A was changed to polyethylene terephthalate resin C. Otherwise, a spunbonded nonwoven fabric was obtained using the same procedure and conditions as in Example 1. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.

[0073] [Example 5] In the fiber spinning process, polyethylene terephthalate resin A was changed to polyethylene terephthalate resin D. Otherwise, a spunbonded nonwoven fabric was obtained using the same procedures and conditions as in Example 1. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.

[0074] [Example 6] In the fiber spinning process, polyethylene terephthalate resin A was changed to polyethylene terephthalate resin C, and polyethylene terephthalate resin B was changed to polyethylene terephthalate resin E. A spunbonded nonwoven fabric was obtained using the same procedures and conditions as in Example 1. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.

[0075] [Example 7] In the step of thermocompression bonding the fiber web, the surface temperature of the hot embossing roll was set to 180°C. Except for this, a spunbonded nonwoven fabric was obtained using the same procedure and conditions as in Example 6. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.

[0076] [Example 8] In the step of thermocompression bonding the fiber web, the surface temperature of the hot embossing roll was set to 190°C. Except for this, a spunbonded nonwoven fabric was obtained using the same procedure and conditions as in Example 6. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.

[0077] Comparative Example 1 In the fiber spinning step, polyethylene terephthalate resin B was replaced with polyethylene terephthalate resin A to form monocomponent fibers. In addition, in the step of thermocompression bonding the fiber web, the surface temperature of the hot embossing roll was set to 250°C. Except for these, a spunbonded nonwoven fabric was obtained using the same procedure and conditions as in Example 1. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.

[0078] Comparative Example 2 In the fiber spinning step, polyethylene terephthalate resin B was replaced with polyethylene terephthalate resin G. Otherwise, a spunbonded nonwoven fabric was obtained using the same procedures and conditions as in Example 1. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.

[0079] Comparative Example 3 In the fiber spinning step, polyethylene terephthalate resin B was changed to polyethylene terephthalate resin F. Otherwise, a spunbonded nonwoven fabric was obtained using the same procedures and conditions as in Example 1. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.

[0080]

[0081] The spunbond nonwoven fabrics of Examples 1 to 8 had high tensile strength and excellent mechanical strength, and also had low tear strength and excellent hand tearability, and exhibited favorable properties as a tape substrate.

[0082] On the other hand, the spunbond nonwoven fabrics of Comparative Examples 1 to 3 had high tear strength and poor hand-tearability (Comparative Examples 1 to 3), or had low tensile strength and insufficient mechanical strength (Comparative Example 1).

[0083] 1: Fibers without sores 2: Fibers with sores 3: Sores

Claims

1. A spunbond nonwoven fabric composed of fibers whose main component is polyethylene terephthalate resin, which has a crystallization peak in the range of 100°C to 150°C and a single melting peak in the range of 250°C to 270°C when measured by differential scanning calorimetry, and has an embossed compression rate of 5% to 30% by area.

2. The spunbond nonwoven fabric according to claim 1, wherein the fiber breakage rate per unit area in the non-bonded parts is 5.0% or more and 50.0% or less.

3. A tape comprising the spunbond nonwoven fabric according to claim 1 or 2.

4. A method for producing the spunbonded nonwoven fabric according to claim 1 or 2, comprising the following steps (a) to (c) in this order: Step (a): A step of spinning out a core-sheath type composite fiber in which a low-viscosity polyethylene terephthalate resin having a melting point of 250°C to 270°C and having an intrinsic viscosity (IV) lower than the intrinsic viscosity (IV) of the high-viscosity polyethylene terephthalate resin by 0.05 to 0.25, is disposed around a high-viscosity polyethylene terephthalate resin having a melting point of 250°C to 270°C. Step (b): A step of drawing and stretching the spun core-sheath type composite fiber by an ejector and depositing it on a moving net conveyor to form a fiber web. Step (c): A step of thermally compressing the fiber web to an embossing compression ratio in the range of 5 area % to 30 area %.

Citation Information

Patent Citations

  • Filament nonwoven fabric and tape of holding and winding electric wire

    JP2007162186A

  • Composite nonwoven fabric for patch

    JP2008163538A

  • Area-bonded nonwoven fabric manufactured from a single polymer system

    JP2010537068A

  • Short-cut fiber for wet-laid nonwoven fabric

    JP2014037644A