Resin composition, cured article, substrate with cured article, laminate, and method for manufacturing semiconductor device
The resin composition with polyimide and specific diamine and acid dianhydride residues addresses the limitations of existing adhesives by providing high heat resistance and durability, and enabling solvent-free cleaning in semiconductor device manufacturing.
Patent Information
- Application Number
- PCT/JP2024/012238
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
Semiconductor devices face challenges with adhesives used in manufacturing, such as warping and damage due to stress changes during heat treatment and thinning processes, and existing adhesives like acrylic and silicone resins have limitations in heat resistance and durability, requiring volatile solvents for cleaning.
A resin composition containing polyimide with specific diamine and acid dianhydride residues, optimized for high heat resistance, durability, and solubility, which suppresses volatile matter generation and allows for cleaning without polar solvents.
The resin composition provides excellent heat resistance, durability, and bonding properties, preventing damage during semiconductor processing and eliminating the need for volatile solvents in cleaning, enhancing the manufacturing efficiency of semiconductor devices.
Smart Images

Figure JP2024012238_03102024_PF_FP_ABST
Abstract
Description
Resin composition, cured product, substrate with cured product, laminate, and method for manufacturing semiconductor device
[0001] The present invention relates to a resin composition, a cured product, a substrate with the cured product, a laminate, and a method for manufacturing a semiconductor device. More specifically, the present invention relates to a resin composition, a cured product, a substrate with the cured product, a laminate, and a method for manufacturing a semiconductor device using the same, which are suitable for bonding a semiconductor element to a supporting substrate.
[0002] In recent years, semiconductor devices have become increasingly smaller and thinner. For example, display semiconductor devices such as mini-LED and micro-LED displays have been proposed, and there is a demand for further miniaturization and thinning in order to improve resolution and reduce costs. In the manufacturing process of these semiconductor devices, semiconductor elements undergo heat treatment and thinning processes, which are prone to warping and damage due to stress changes. Therefore, adhesives are used to improve handling. That is, the semiconductor element, which is the workpiece, is bonded to a support substrate using an adhesive, and after going through a series of manufacturing processes, it is peeled off from the support substrate by laser peeling or the like.
[0003] Natural rubber and styrene-butadiene rubber are commonly used as adhesives for general purposes, but temporary adhesives for semiconductor device processing require high heat resistance, so acrylic resins and silicone resins have been used.
[0004] Acrylic resins are highly transparent and are widely used as optical materials for flat panel displays such as liquid crystal panels (see, for example, Patent Document 1), but have insufficient heat resistance because the acrylic resins decompose when left at high temperatures of 200° C. or higher for a long period of time. Silicone resins exhibit higher heat resistance than acrylic resins (see, for example, Patent Document 2), but have the problem of generating low-molecular-weight volatile components when left at high temperatures of 250° C. or higher for a long period of time, which can cause poor conductivity in semiconductor devices.
[0005] Polyimide is an example of a resin that exhibits heat resistance of 250° C. or higher. As a polyimide for use as a temporary adhesive, polyimidesiloxanes that have a glass transition temperature of 200° C. or lower by copolymerizing polysiloxane-based diamines have been proposed (e.g., Patent Documents 3, 4, and 5).
[0006] Patent Document 1: JP 2008-308549 A Patent Document 2: JP 2005-105246 A Patent Document 3: WO 2013 / 039029 Patent Document 4: JP 2019-172894 A Patent Document 5: JP 2003-327697 A
[0007] However, while polyimidesiloxanes containing a large amount of flexible polysiloxane components, such as those disclosed in Patent Documents 3 and 4, have excellent lamination properties, there is room for improvement in durability during thinning and heat treatment processes of semiconductor elements.
[0008] On the other hand, polyimidesiloxanes having aromatic diamines with a linear aliphatic chain, as disclosed in Patent Document 5, have sufficiently high glass transition temperatures and elastic moduli, and therefore have excellent durability in heat treatment and thinning processes, but are inferior in lamination properties.
[0009] Furthermore, when using the polyimidesiloxane adhesive, a highly polar solvent must be used to clean off the residue remaining on the semiconductor chip after laser peeling, which necessitates a rinsing step using a volatile solvent, increasing the number of steps.
[0010] Therefore, there has been a strong demand for a resin composition, a cured product, a substrate with the cured product, a laminate, and a method for manufacturing a semiconductor device using these, which can solve the problems of the conventional techniques as described above and are suitable for use as an adhesive in manufacturing a semiconductor device.
[0011] The present invention addresses the problem of providing a resin composition, a cured product, and a laminate that are suitable for use as adhesives in the manufacture of semiconductor devices, which do not generate volatile matter due to decomposition even in high-temperature environments, have excellent lamination properties, are excellent in durability in heat treatment and thinning processes, and can be cleaned without using highly polar solvents after laser peeling, as well as a method for manufacturing a semiconductor device using these.
[0012] The present invention and its preferred embodiments for solving the above problems comprise the following: [1] A resin composition containing a polyimide-containing resin (A) and a solvent, wherein the resin (A) contains a diamine residue (a1) represented by formula (1) and a diamine residue (a2) represented by formula (2), wherein, based on 100.0 mol% of all diamine residues in the resin (A), the content of the diamine residue (a1) is 30.0 mol% or more but less than 50.0 mol%, and the content of the diamine residue (a2) is 30.0 mol% or more but 70.0 mol% or less, and the content of Si atoms contained in the resin (A) is 12.0 mol% or more but 16.0 mol% or less, based on 100.0 mol% of the resin (A).
[0013]
[0014] In formula (1), R 1 ~R 4 R each independently represents an alkyl group having 1 to 30 carbon atoms, a phenyl group, or a phenoxy group. 5 and R 6 each independently represents an alkylene group or a phenylene group having 1 to 30 carbon atoms, and n represents a range of 5 to 30. * represents the bonding site to the nitrogen atom in the imide group.
[0015]
[0016] In formula (2), R 7 ~R 14 each independently represent a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, a hydroxyl group, or a halogen. * represents a bonding site to a nitrogen atom in an imide group. [2] The resin composition according to [1], wherein the molar ratio of the content of diamine residues (a2) to the content of diamine residues (a1) in resin (A) is 0.9 to 1.6. [3] The resin composition according to [1] or [2], wherein resin (A) contains 50.0 mol % or more and 100.0 mol % or less of acid dianhydride residues (a3) represented by formula (3) relative to 100.0 mol % of all acid anhydride residues in resin (A).
[0017]
[0018] In formula (3), R 15 is a single bond, -C(H2 )-, -O-, -C(O)-, -C(CH 3 ) 2 -, -S(O 2 ) -, -C(CF 3 ) 2 -, and R 16 ~R 21 each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, a hydroxyl group, or a halogen. * represents a bonding site to a carbon atom in an imide group. [4] When the resin (A) contains 100.0 mol% of the total acid dianhydride residues (a3), R in formula (3) 15 -C(CF 3 ) 2 [5] The resin composition according to [3], wherein the ratio of R in formula (3) to the content of the acid dianhydride residue (a3-1) in the resin (A) is 20.0 mol % or more and less than 80.0 mol %. 15 [6] The resin composition according to any one of [1] to [5], wherein the resin (A) further contains a diamine residue (a5) represented by formula (5), and the content of the diamine residue (a5) in 100.0 mol % of all diamine residues in the resin (A) is 10.0 mol % or more and 30.0 mol % or less.
[0019]
[0020] In formula (5), R 22 ~R 29 each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, a hydroxyl group, or a halogen atom. * represents a bonding site to a carbon atom in the imide group. [7] The resin composition according to [6], wherein the diamine residue (a5) is a diamine residue having a structure represented by formula (6):
[0021]
[0022] In formula (6), * represents a bonding site to a carbon atom in the imide group. [8] The resin composition according to any one of [1] to [7], wherein the weight-average molecular weight of resin (A) is 10,000 or more and 30,000 or less. [9] A cured product derived from the resin composition according to any one of [1] to [8].
[10] The cured product according to [9], wherein the dissolution rate in acetone is 100 nm / min or more and less than 10,000 nm / min.
[11] The cured product according to [9] or
[10] , wherein the storage modulus at 200°C is 0.5 MPa or more and less than 5.0 MPa.
[12] A substrate with a cured product, in which the cured product according to any one of [9] to
[11] is formed on a supporting substrate.
[13] A laminate in which a semiconductor element is laminated on the substrate with the cured product according to
[12] .
[14] A method for manufacturing a semiconductor device, in which the resin composition according to any one of [1] to [8] is used.
[15] A method for manufacturing a semiconductor device, in which the cured product according to any one of [9] to
[11] is used.
[16] A method for manufacturing a semiconductor device, using a substrate with a cured product according to
[12] .
[17] A method for manufacturing a semiconductor device, using a laminate according to
[13] .
[0023] According to the present invention, the resin composition of the present invention has excellent heat resistance, so that the generation of volatile matter due to decomposition can be suppressed even in high-temperature environments. Furthermore, because it has a moderate elastic modulus at high temperatures, it has excellent lamination properties and excellent durability in the thinning process and heat treatment process. Furthermore, because it can be cleaned without using a highly polar solvent after laser peeling, the rinsing process using a volatile solvent can be omitted.
[0024] Fig. 1 is a schematic cross-sectional view showing the first half of an example of a manufacturing process for a semiconductor device of the present invention; Fig. 2 is a schematic cross-sectional view showing the second half of an example of a manufacturing process for a semiconductor device of the present invention; Fig. 3 is a schematic cross-sectional view showing the first half of another example of a manufacturing process for a semiconductor device of the present invention; Fig. 4 is a schematic cross-sectional view showing the second half of another example of a manufacturing process for a semiconductor device of the present invention.
[0025] The present invention will be described in detail below.
[0026] <Polyimide-containing resin (A)> The resin composition of the present invention contains a polyimide-containing resin (A). The polyimide-containing resin in the present invention is a resin containing a polyimide, a polyimide precursor, or a copolymer thereof.
[0027] Polyimide is a resin having a cyclic structure of imide rings in the main chain structure. Polyimide precursors are resins that form imide rings by dehydration ring closure, and examples thereof include polyamic acid and polyamic acid ester.
[0028] Polyimides can be obtained by reacting tetracarboxylic acids, corresponding tetracarboxylic dianhydrides, tetracarboxylic diester dichlorides, etc. with diamines, corresponding diisocyanate compounds, trimethylsilylated diamines, etc., and contain organic groups derived from the acid dianhydrides, i.e., acid dianhydride residues, and organic groups derived from the diamines, i.e., diamine residues. Polyimides can be obtained, for example, by dehydrating and cyclizing polyamic acids obtained by reacting tetracarboxylic dianhydrides with diamines in the presence or absence of a solvent, followed by heat treatment. A solvent that forms an azeotrope with water, such as m-xylene, may be added during this heat treatment. Alternatively, polyimides can be obtained by adding a dehydrating and cyclizing catalyst, such as a carboxylic anhydride, a dehydrating condensing agent, such as dicyclohexylcarbodiimide, or a base, such as triethylamine, followed by chemical heat treatment. Alternatively, polyimides can be obtained by adding a weakly acidic carboxylic acid compound and then heat treatment at a low temperature of 100°C or below to dehydrate and cyclize the polyamic acid.
[0029] Examples of solvents used in polyimide polymerization include polar aprotic solvents such as N-methyl-2-pyrrolidone, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, and dimethyl sulfoxide, ether solvents such as tetrahydrofuran, dioxane, and propylene glycol monomethyl ether, ketone solvents such as acetylacetone, methyl ethyl ketone, methyl propyl ketone, methyl butyl ketone, diisobutyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, and 2-heptanone, ester solvents such as ethyl acetate, propylene glycol monomethyl ether acetate, and ethyl lactate, and aromatic hydrocarbon solvents such as toluene and xylene. These may be used alone or in combination of two or more.
[0030] The resin (A) contains a diamine residue (a1) represented by formula (1).
[0031]
[0032] In formula (1), R 1 ~R 4 R each independently represents an alkyl group having 1 to 30 carbon atoms, a phenyl group, or a phenoxy group. 5 and R 6 each independently represents an alkylene group or a phenylene group having 1 to 30 carbon atoms, and n represents a range of 5 to 30. * represents the bonding site to the nitrogen atom in the imide group.
[0033] When n in formula (1) is 5 or more, the Si content in the resin (A) is increased, resulting in high adhesiveness. Furthermore, when n is 30 or less, the compatibility between the diamine residue (a1) and other monomers is improved during polymerization of the resin (A), facilitating the reaction and resulting in a sufficient molecular weight. More preferably, n is 10 or less. With n in this range, Si can be dispersed and present in the resin (A), resulting in uniform adhesiveness in the coating film. The n represents an average value, and the average value of n can be calculated from the average molecular weight of the diamine residue (a1). The average molecular weight of the diamine residue (a1) can be determined by calculating the amino group equivalent by neutralization titration of the amino groups of the siloxane diamine and then doubling this amino group equivalent. For example, a predetermined amount of diamine residue (a1) is collected and placed in a beaker, and dissolved in a 1:1 mixture of isopropyl alcohol (hereinafter referred to as IPA) and toluene. A predetermined concentration of hydrochloric acid is then added dropwise to the solution. The amino group equivalent can be calculated from the amount of hydrochloric acid added at the neutralization point. Doubling this amino group equivalent gives the average molecular weight. Separately, the molecular weights of the diamine residue (a1) used in titration when n = 1 and when n = 10 can be calculated from the chemical structural formula, and the relationship between the value of n and the molecular weight can be obtained as a linear equation. Substituting the average molecular weight into this equation allows the average value of n to be obtained.
[0034] Examples of diamines that provide the diamine residue (a1) include α,ω-bis(3-aminopropyl)polydimethylsiloxane, α,ω-bis(3-aminopropyl)polydiethylsiloxane, α,ω-bis(3-aminopropyl)polydipropylsiloxane, α,ω-bis(3-aminopropyl)polydibutylsiloxane, α,ω-bis(3-aminopropyl)polydiphenoxysiloxane, α,ω-bis(2-aminoethyl)polydimethylsiloxane, α,ω-bis(2 α,ω-bis(4-aminoethyl)polydiphenoxysiloxane, α,ω-bis(4-aminobutyl)polydimethylsiloxane, α,ω-bis(4-aminobutyl)polydiphenoxysiloxane, α,ω-bis(5-aminopentyl)polydimethylsiloxane, α,ω-bis(5-aminopentyl)polydiphenoxysiloxane, α,ω-bis(4-aminophenyl)polydimethylsiloxane, α,ω-bis(4-aminophenyl)polydiphenoxysiloxane, etc. These may be used alone or in combination of two or more.
[0035] The content of diamine residue (a1) is 30.0 mol% or more and less than 50.0 mol%, preferably 35.0 mol% or more and 45.0 mol% or less, of the total diamine residues in resin (A) being 100.0 mol%. If the content of diamine residue (a1) is less than 30.0 mol%, the lamination property is poor, and if the content of diamine residue (a1) is 50.0 mol% or more, the elastic modulus of resin (A) at high temperatures is poor, and the durability in the thinning step and the heat treatment step is poor.
[0036] The resin (A) also contains a diamine residue (a2) represented by formula (2).
[0037]
[0038] In formula (2), R 7 ~R 14 each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, a hydroxyl group, or a halogen. * represents the bonding site to the nitrogen atom in the imide group.
[0039] Examples of diamines that provide the diamine residue (a2) include 3,3'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, bis(3-amino-4-hydroxyphenyl) sulfone, bis(4-amino-3-hydroxyphenyl) sulfone, etc. These may be used alone or in combination of two or more.
[0040] The content of diamine residue (a2) is 30.0 mol% or more and 70.0 mol% or less, where the total diamine residues in resin (A) is 100.0 mol%. When the content of diamine residue (a2) is 30.0 mol% or more, preferably 35.0% or more, the resin (A) has excellent solubility in acetone and excellent cleanability. When the content of diamine residue (a2) is 70.0 mol% or less, preferably 65.0% or less, the resin (A) has a sufficient content of diamine residue (a1), resulting in excellent lamination properties.
[0041] The molar ratio of the content of the diamine residue (a2) to the content of the diamine residue (a1) in the resin (A) is preferably 0.9 to 1.6, which allows the dissolution rate in acetone and the lamination properties to be more effectively optimized.
[0042] The resin (A) preferably further contains a diamine residue (a5) represented by formula (5).
[0043]
[0044] In formula (5), R 22 ~R 29 each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, a hydroxyl group, or a halogen atom. * represents the bonding site to a carbon atom in the imide group.
[0045] Examples of diamines that provide the diamine residue (a5) represented by formula (5) include 4,4'-biphenyldiamine, 2,2'-dimethylbiphenyl-4,4'-diamine, 4,4'-diamino-3,3',5,5'-tetramethylbiphenyl, 4,4'-diamino-3,3'-dimethylbiphenyl, 2,2'-benzidinedisulfonic acid, 4,4'-diamino-2,2'-bis(trifluoromethyl)biphenyl, 4,4'-diamino-3,3'-diethylbiphenyl dihydrochloride, octafluorobenzidine, 4,4'-diamino-3,3'-dimethoxybiphenyl, etc. These may be used alone or in combination of two or more.
[0046] When the resin (A) contains the diamine residue (a5), more preferably the diamine residue having the structure represented by formula (6), the resin (A) has excellent solvent solubility and can be uniformly applied, resulting in excellent lamination properties.
[0047]
[0048] In formula (6), * represents the bonding site to the carbon atom in the imide group.
[0049] An example of a diamine that provides a diamine residue having the structure represented by formula (6) is 2,2'-dimethylbiphenyl-4,4'-diamine.
[0050] The content of the diamine residue (a5) in the resin (A) is preferably 10.0 mol % or more and 30.0 mol % or less, based on 100.0 mol % of all diamine residues. By having the content of the diamine residue (a5) within the above range, the elastic modulus at high temperatures can be appropriately adjusted, and the lamination property and durability in the thinning step and heat treatment step can be effectively improved.
[0051] The resin (A) may contain a diamine residue other than the diamine residue (a1), the diamine residue (a2), and the diamine residue (a5). Examples of diamines that provide diamine residues other than the diamine residue (a1), the diamine residue (a2), and the diamine residue (a5) include 4,4'-bis(4-aminophenoxy)biphenyl, p-phenylenediamine, m-phenylenediamine, 2,5-diaminotoluene, 2,4-diaminotoluene, 3,5-diaminobenzoic acid, 2,6-diaminobenzoic acid, 2-methoxy-1,4-phenylenediamine, 4,4'-diaminobenzanilide, 3,4'-diaminobenzanilide, 3,3'-diaminobenzanilide, 3, 3'-Dimethyl-4,4'-diaminobenzanilide, 9,9-bis(4-aminophenyl)fluorene, 9,9-bis(3-aminophenyl)fluorene, 9,9-bis(3-methyl-4-aminophenyl)fluorene, 9,9-bis(3,5-dimethyl-4-aminophenyl)fluorene, 9,9-bis(3-methoxy-4-aminophenyl)fluorene, 9,9-bis(4-aminophenyl)fluorene-4-carboxylic acid, 9,9-bis(4-aminophenyl)fluorene-4-methyl, 9,9-bis(4-aminophenyl)fluorene 9,9-bis(4-aminophenyl)fluorene-4-methoxy, 9,9-bis(4-aminophenyl)fluorene-4-ethyl, 9,9-bis(4-aminophenyl)fluorene-3-carboxylic acid, 9,9-bis(4-aminophenyl)fluorene-3-methyl, 1,3-diaminocyclohexane, 2,2'-dimethylbenzidine, 3,3'-dimethylbenzidine, 3,3'-dimethoxybenzidine, 2,4-diaminopyridine, 2,6-diaminopyridine, 1,5-diaminonaphthalene, 2,7-diaminofluorene, p-aminobenzylamine, m-Aminobenzylamine, 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 3,3'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 3,3'-diaminobenzophenone, 3,4'-diaminobenzophenone, 4,4'-diaminobenzophenone, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 1,3-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 1,4-bis(3-aminophenoxy)benzene, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(3-aminophenoxy)phenyl]propane, bis[4-(4-aminophenoxy)phenyl]methane, bis[4-(3-aminophenoxy)phenyl]methane, bis[4-(4-aminophenoxy)phenyl] bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 1,4-diaminocyclohexane, 4,4'-methylenebis(cyclohexylamine), 3,3'-methylenebis(cyclohexylamine), 4,4'-diamino-3,3'-dimethyldicyclohexylmethane, 4,4'-diamino-3,3'-dimethyldicyclohexyl, etc. These may be used alone or in combination of two or more.
[0052] The resin (A) preferably contains an acid dianhydride residue (a3) represented by formula (3).
[0053]
[0054] In formula (3), R 15 is a single bond, -C(H 2 )-, -O-, -C(O)-, -C(CH 3 ) 2 -, -S(O 2 ) -, -C(CF 3 ) 2 -, and R 16 ~R 21 Each of the symbols independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, a hydroxyl group, or a halogen. * represents the bonding site to a carbon atom in the imide group.
[0055] Examples of acid dianhydrides that provide the acid dianhydride residue (a3) include 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,2'dimethyl-3,3',4,4'-biphenyltetracarboxylic dianhydride, 5,5'dimethyl-3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-diphenylethertetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 3,3',4,4'-diphenylmethylenetetracarboxylic dianhydride, 4,4'-isopropylidenediphthalic dianhydride, 4,4'-(hexafluoroisopropylidene)diphthalic dianhydride, 4,4'-oxydiphthalic anhydride, etc. These may be used alone or in combination of two or more.
[0056] The content of the acid dianhydride residue (a3) is preferably 50.0 mol % or more and 100.0 mol % or less, where 100.0 mol % of all acid dianhydride residues in the resin (A) is 1. When the content of the acid dianhydride residue (a3) is within the above range, the elastic modulus at high temperatures can be appropriately adjusted, and the lamination property and durability in the thinning step and heat treatment step can be effectively improved.
[0057] The resin (A) contains 100.0 mol% of the total acid dianhydride residues (a3) of R in formula (3). 15 -C(CF 3 ) 2 When the content of the acid dianhydride residue (a3-1) is within the above range, a sufficient dissolution rate in acetone can be obtained, and cleaning properties can be effectively improved.
[0058] The ratio of R in formula (3) to the content of the acid dianhydride residue (a3-1) in the resin (A) 15 The molar ratio of the content of the acid dianhydride residue (a3-2) in which is —O— is preferably 0.97 to 1.02. When the molar ratio is within this range, the dissolution rate in acetone and durability in the thinning step and heat treatment step can be more effectively optimized.
[0059] Examples of acid dianhydrides that provide the acid dianhydride residue (a3-1) include 4,4'-(hexafluoroisopropylidene)diphthalic dianhydride, etc. These may be used alone or in combination of two or more.
[0060] Examples of the acid dianhydride that gives the acid dianhydride residue (a3-2) include 4,4'-oxydiphthalic anhydride, etc. The acid dianhydrides that give the acid dianhydride residue (a3-2) may be used alone or in combination of two or more.
[0061] The resin (A) may contain an acid dianhydride residue other than the acid dianhydride residue (a3). Examples of acid dianhydrides that provide an acid dianhydride residue other than the acid dianhydride residue (a3) include pyromellitic dianhydride, 3,4,9,10-perylenetetracarboxylic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 3,3",4,4"-para-terphenyltetracarboxylic dianhydride, 3,3",4,4"-meta-terphenyltetracarboxylic dianhydride, 2,3,6,7-anthracenetetracarboxylic dianhydride, and 1,2,7,8-phenanthrenetetracarboxylic dianhydride. tetracarboxylic dianhydride, 2,3,5-tricarboxycyclopentylacetic dianhydride, 1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,2,3,4-cyclopentanetetracarboxylic dianhydride, 1,2,3,5-cyclopentanetetracarboxylic dianhydride, 1,2,4,5-bicyclohexenetetracarboxylic dianhydride, 1,2,4,5-cyclohexanetetracarboxylic dianhydride, 1,3,3a,4,5,9b-hexahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)-naphtho[1,2-C]furan-1,3-dione, etc. These may be used alone or in combination of two or more.
[0062] Resin (A) contains Si atoms, and the content of Si atoms contained in resin (A) is 12.0 mass% or more and 16.0 mass% or less, preferably 13.0 mass% or more and 15.0 mass% or less, based on 100.0 mass% of resin (A). If the proportion of Si atoms is less than 12.0 mass%, the lamination property is poor. If the proportion of Si atoms is 16.0 mass% or more, the elastic modulus of resin (A) at high temperatures is poor, and the durability in the thinning process and heat treatment process is poor. The proportion of Si atoms contained in resin (A) can be calculated from the amount of monomer charged or determined by elemental analysis of resin (A).
[0063] The molar ratio of diamine residues to acid dianhydride residues in resin (A) is preferably 95.0 / 100.0 to 100.0 / 95.0. The molecular weight of resin (A) can be controlled by the molar ratio of diamine residues to acid dianhydride residues, and by setting the molar ratio of diamine residues to acid dianhydride residues within the above range, it is possible to prevent the molecular weight of resin (A) from becoming smaller and thereby prevent a decrease in the elastic modulus of the cured product.
[0064] It is also preferable that the resin (A) is end-capped with one or more of a monoamine, an acid anhydride, an acid chloride, and a monocarboxylic acid, since the resin composition has excellent storage stability when the end-capped with one or more of a monoamine, an acid anhydride, an acid chloride, and a monocarboxylic acid.
[0065] When the terminals are blocked with the monoamine, the amount of the monoamine is preferably in the range of 0.1 to 60.0 mol% based on the total amine components. Excellent storage stability is achieved when the amount of the monoamine is 0.1 mol% or more, more preferably 5 mol% or more. Furthermore, a sufficient weight-average molecular weight can be obtained when the amount of the monoamine is 60.0 mol% or less, more preferably 50.0 mol% or less.
[0066] Examples of the monoamine include 5-amino-8-hydroxyquinoline, 1-hydroxy-7-aminonaphthalene, 1-hydroxy-6-aminonaphthalene, 1-hydroxy-5-aminonaphthalene, 1-hydroxy-4-aminonaphthalene, 2-hydroxy-7-aminonaphthalene, 2-hydroxy-6-aminonaphthalene, 2-hydroxy-5-aminonaphthalene, 1-carboxy-7-aminonaphthalene, 1-carboxy-6-aminonaphthalene, and 1-carboxy-5-aminonaphthalene. , 2-carboxy-7-aminonaphthalene, 2-carboxy-6-aminonaphthalene, 2-carboxy-5-aminonaphthalene, 2-aminobenzoic acid, 3-aminobenzoic acid, 4-aminobenzoic acid, 4-aminosalicylic acid, 5-aminosalicylic acid, 6-aminosalicylic acid, 3-amino-4,6-dihydroxypyrimidine, 2-aminophenol, 3-aminophenol, 4-aminophenol, 2-aminothiophenol, 3-aminothiophenol, 4-aminothiophenol, etc. These may be used alone or in combination of two or more.
[0067] When the terminals are blocked with the acid anhydride, acid chloride, or monocarboxylic acid, the total amount of these compounds is preferably in the range of 0.1 to 60.0 mol % relative to the total acid components. Excellent storage stability can be achieved by using an amount of 0.1 mol % or more, more preferably 5.0 mol % or more, and a sufficient weight-average molecular weight can be achieved by using an amount of 60.0 mol % or less, more preferably 50.0 mol % or less.
[0068] Examples of acid anhydrides, acid chlorides, and monocarboxylic acids include acid anhydrides such as phthalic anhydride, maleic anhydride, nadic anhydride, cyclohexanedicarboxylic anhydride, and 3-hydroxyphthalic anhydride, 3-carboxyphenol, 4-carboxyphenol, 3-carboxythiophenol, 4-carboxythiophenol, 1-hydroxy-7-carboxynaphthalene, 1-hydroxy-6-carboxynaphthalene, 1-hydroxy-5-carboxynaphthalene, 1-mercapto-7-carboxynaphthalene, 1-mercapto-6-carboxynaphthalene, and 1-mercapto-5-carboxynaphthalene. monoacid chloride compounds in which only one carboxy group of dicarboxylic acids such as terephthalic acid, phthalic acid, maleic acid, cyclohexanedicarboxylic acid, 1,5-dicarboxynaphthalene, 1,6-dicarboxynaphthalene, 1,7-dicarboxynaphthalene, and 2,6-dicarboxynaphthalene is acid chlorided, and activated ester compounds obtained by reacting a monoacid chloride compound with N-hydroxybenzotriazole or N-hydroxy-5-norbornene-2,3-dicarboximide. These may be used alone or in combination of two or more.
[0069] The weight average molecular weight of the resin (A) is preferably 10,000 or more and 30,000 or less, more preferably 15,000 or more and 25,000 or less. When the weight average molecular weight is 10,000 or more, more preferably 15,000 or more, the elastic modulus of the cured product is excellent. Furthermore, when the weight average molecular weight is 30,000 or less, more preferably 25,000 or less, the resin has excellent solubility in moderate acetone. The weight average molecular weight is measured by gel permeation chromatography (GPC) and calculated in terms of polystyrene.
[0070] The resin (A) preferably has a dispersity of 2.0 or more and 3.0 or less. A dispersity of 2.0 or more, more preferably 2.2 or more, increases the dissolution rate of the resin (A) in acetone, resulting in excellent cleanability. A dispersity of 3.0 or less, more preferably 2.8 or less, can suppress low molecular weight components, resulting in excellent elastic modulus of the cured product. The dispersity is measured by gel permeation chromatography (GPC) and is expressed as Mw / Mn, using the weight average molecular weight (Mw) and number average molecular weight (Mn) calculated in terms of polystyrene.
[0071] <Solvent> The resin composition of the present invention contains a solvent. The solvent in the present invention refers to a component capable of dissolving the resin (A) and other components.
[0072] The content of the solvent is not particularly limited, but is preferably 100.0 parts by mass or more and 2000.0 parts by mass or less relative to 100.0 parts by mass of the resin (A). When the content of the solvent is 100.0 parts by mass, the resin (A) can be sufficiently dissolved, resulting in excellent coatability and flatness of the coating film. When the content is 2000 parts by mass or less, the decrease in viscosity is suppressed and a film thickness of 1 μm or more can be formed.
[0073] Examples of the solvent include polar aprotic solvents such as N-methyl-2-pyrrolidone, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, and dimethyl sulfoxide; ether solvents such as tetrahydrofuran, dioxane, and propylene glycol monomethyl ether; ketone solvents such as acetylacetone, methyl ethyl ketone, methyl propyl ketone, methyl butyl ketone, diisobutyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, and 2-heptanone; ester solvents such as ethyl acetate, propylene glycol monomethyl ether acetate, and ethyl lactate; and aromatic hydrocarbon solvents such as toluene and xylene. These solvents may be used alone or in combination of two or more. Furthermore, the solvent used as the polymerization solvent for resin (A) may be used as a solvent without being removed from the solution after polymerization.
[0074] <Other Components> In addition to the resin (A) and the solvent, the resin composition of the present invention may contain other components within the scope of not impairing the effects of the present invention. Examples of other components include other resins, crosslinking agents, silane coupling agents, fillers, etc.
[0075] Examples of other resins include acrylic resins, acrylonitrile resins, butadiene resins, urethane resins, polyester resins, polyamide resins, polyamideimide resins, epoxy resins, phenolic resins, etc. These may be used alone or in combination of two or more.Examples of the crosslinking agent include compounds having one or more organic groups selected from an epoxy group, a methylol group, and an alkoxymethyl group, such as ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, tripropylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, and glycerin diglycidyl. ether, 2,2-dibromoneopentyl glycol diglycidyl ether, 1,3,5,,6-tetraglycidyl-2,4-hexanediol, N,N,N',N'-tetraglycidyl-m-xylenediamine, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, N,N,N',N'-tetraglycidyl-4,4'-diaminodiphenylmethane, N,N,-diglycidyl-benzylamine, N,N-diglycidyl-benzylamine, N,N-diglycidyl-aminomethylcyclohexane, Commercially available products include MX-750, which has an average of 3.7 methoxymethyl groups substituted per triazine ring, MW-30 and MX-100LM, which have an average of 5.8 methoxymethyl groups substituted per triazine ring (all manufactured by Sanwa Chemical Co., Ltd.), methoxymethylated melamines such as Cymel 300, 301, 303, 350, 370, 771, 325, 327, 703 and 712, methoxymethylated butoxymethylated melamines such as Cymel 235, 236, 238, 212, 253 and 254, and butoxymethylated melamines such as Cymel 506 and 508. Examples include methylated melamine, carboxyl group-containing methoxymethylated isobutoxymethylated melamine such as Cymel 1141, methoxymethylated ethoxymethylated benzoguanamine such as Cymel 1123, methoxymethylated butoxymethylated benzoguanamine such as Cymel 1123-10, butoxymethylated benzoguanamine such as Cymel 1128, and carboxyl group-containing methoxymethylated ethoxymethylated benzoguanamine such as Cymel 1125-80 (all manufactured by Mitsui Cyanamid Co., Ltd.). These may be used alone or in combination of two or more.
[0076] Examples of silane coupling agents include vinyltrimethoxysilane, vinyltriethoxysilane, epoxycyclohexylethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, p-styryltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, etc. These may be used alone or in combination of two or more.
[0077] Examples of fillers include silica, alumina, titanium oxide, quartz powder, magnesium carbonate, potassium carbonate, barium sulfate, mica, talc, etc. These may be used alone or in combination of two or more.
[0078] <Cured Product> The cured product of the present invention is a cured product obtained by curing the resin composition. That is, the cured product of the present invention is derived from the resin composition of the present invention. The cured product referred to here may be in any form as long as the resin composition is cured by heat. Examples of a method for curing by heat include a method of curing by heat treatment at 150°C or higher and 500°C or lower for 5 minutes to 5 hours.
[0079] The method for producing the cured product includes the steps of applying the resin composition onto a substrate and drying it to form a resin film on the substrate, and curing the resin film by heat treatment.
[0080] Examples of the process of applying the resin composition onto a substrate and drying it to form a resin film on the substrate include a process of applying the resin composition onto a substrate using a spin coater, spray coater, screen coater, blade coater, die coater, calendar coater, meniscus coater, bar coater, roll coater, comma roll coater, gravure coater, slit die coater, or the like, and drying it using an oven, a hot plate, infrared rays, or the like at a temperature in the range of 50°C to 150°C for 1 minute to 24 hours to form a resin film.
[0081] Examples of the process of heat-treating and curing the resin film include a process of heat-treating the resin film at 150°C to 500°C for 5 minutes to 5 hours using an oven, a hot plate, infrared rays, or the like. The heat treatment can be performed by selecting a temperature and gradually increasing the temperature, or by selecting a temperature range and continuously increasing the temperature. An example of the former is a method of heat-treating the resin film at 200°C and 250°C for 30 minutes each. An example of the latter is a method of increasing the temperature from room temperature to 250°C over 1 hour.
[0082] The cured product of the present invention preferably has a dissolution rate in acetone of 100 nm / min or more and less than 10,000 nm / min. When the dissolution rate is 100 nm / min or more, more preferably 150 nm / min or more, and even more preferably 5,000 nm / min or more, the cured product formed on the substrate can be washed with acetone, a volatile solvent. In other words, when washing the residue of the cured product remaining on the semiconductor chip after laser peeling, there is no need to use a highly polar solvent, and a rinsing step with a volatile solvent is not required. When the dissolution rate in acetone is 10,000 nm / min or less, excellent cleanability can be achieved without impairing resistance to chemicals other than acetone.
[0083] The dissolution rate in acetone can be determined from the change in film thickness when a cured product formed on a substrate is treated with acetone. Specifically, the film thickness of the cured product formed on a substrate before being treated with acetone is T 1 (nm), the film thickness after treatment with acetone by immersing the cured product in acetone at 25°C for 10 minutes was T 2 (nm), (T 1 -T 2 ) / 10 (nm / min).
[0084] The cured product of the present invention preferably has a 1% weight loss temperature of 400° C. or higher and 500° C. or lower. Having a 1% weight loss temperature within this preferred range is advantageous in that generation of volatile matter due to decomposition can be suppressed even in a high-temperature environment.
[0085] The 1% weight loss temperature can be determined by thermogravimetric analysis (TGA). Specifically, 15 mg of the cured product is placed in a TGA apparatus and maintained at 120°C for 30 minutes in a nitrogen atmosphere to remove moisture from the cured product, followed by heating to 500°C at a rate of 5°C / min. The 1% weight loss temperature can be determined from the resulting weight loss curve.
[0086] The cured product of the present invention preferably has a glass transition temperature of 100° C. or higher and 200° C. or lower. A glass transition temperature within this preferred range is preferred in that it provides excellent lamination properties and durability in the thinning step and heat treatment step.
[0087] The glass transition temperature can be determined by thermomechanical analysis (TMA). Specifically, a 10 μm thick freestanding film of the cured product is prepared, cut into a 3 cm × 1.5 cm cylindrical sample, and subjected to indentation TMA measurement. The glass transition temperature can be determined from the inflection point in the obtained temperature-expansion curve.
[0088] The cured product of the present invention preferably has a storage modulus of 0.5 MPa or more and 5 MPa or less at 200°C. By having the storage modulus of 0.5 MPa or more, more preferably 1.0 MPa or less, durability in the thinning step and heat treatment step can be more effectively obtained. By having the storage modulus of 5.0 MPa or less at 200°C, excellent lamination properties can be achieved.
[0089] The storage modulus at 200°C can be determined by dynamic mechanical analysis (DMA) or nanoindenter measurement. Specifically, in the case of DMA, a free-standing film of the cured product having a thickness of 50 μm is prepared, and the storage modulus at 200°C can be determined by measurement using a tension method at 25°C to 250°C and a frequency of 1 Hz. In the case of nanoindenter measurement, the cured product is prepared on a substrate having a thickness of 10 μm, and the storage modulus at 200°C can be determined by measurement using an indentation method at 25°C to 250°C and a frequency of 1 Hz.
[0090] <Substrate with Cured Product> The substrate with cured product of the present invention is a substrate with cured product in which the cured product is formed on a supporting substrate.
[0091] Examples of the support substrate include a silicon substrate, a glass substrate, a quartz substrate, a sapphire substrate, a ceramic substrate, a metal substrate, and a semiconductor substrate.
[0092] The film thickness of the cured product in the substrate with the cured product is preferably 1 to 50 μm, more preferably 5 to 30 μm. When the film thickness of the cured product is in this preferred range, the semiconductor element can be reliably held by the cured product, and the semiconductor element can be prevented from being embedded in the cured product when the semiconductor element and the substrate with the cured product are bonded together.
[0093] The film thickness of the cured product on the substrate with the cured product can be measured using an optical film thickness meter, a scanning electron microscope, a step gauge, a laser microscope, or the like.
[0094] <Laminate> The laminate of the present invention is a laminate in which a semiconductor element is laminated on the substrate with the cured product. More specifically, it is a laminate in which a semiconductor element is laminated in contact with the cured product of the substrate with the cured product, and the surface of the semiconductor element in contact with the cured product is the surface opposite to the surface of the cured product in contact with the supporting substrate.
[0095] Examples of semiconductor elements include those formed by fabricating semiconductors such as GaN, AlN, InN, InP, GaAs, Si, and SiC. These semiconductor elements also include those in which different types of semiconductors are stacked, those in which electrode materials or substrates are stacked, and packaged elements. The size of the semiconductor element is not limited, and multiple elements may be held on the cured product.
[0096] Examples of methods for laminating semiconductor elements onto a substrate with a cured product include bonding a semiconductor substrate before element formation to a substrate with a cured product using a wafer bonder or the like, and then thinning or cutting the semiconductor substrate into small pieces on the substrate with the cured product. Another method includes bonding semiconductor elements previously fabricated on a separate substrate to the substrate with the cured product using a wafer bonder or the like, and then removing the separate substrate. Another method includes transferring the semiconductor elements one by one onto the substrate with the cured product using a flip-chip bonder or the like. In this case, it is preferable to bond the semiconductor elements while heating at a temperature equal to or higher than the glass transition temperature of the cured product. Heating the bonding at a temperature equal to or higher than the glass transition temperature is preferable because it reduces the elastic modulus of the cured product and ensures that the semiconductor elements are securely held in place.
[0097] <Method for manufacturing a semiconductor device> The method for manufacturing a semiconductor device of the present invention is a method for manufacturing a semiconductor device using the resin composition, the cured product, the substrate with the cured product, or the laminate. As an example of the method for manufacturing a semiconductor device of the present invention, a method for manufacturing a mini LED display will be described with reference to the drawings.
[0098] 1 and 2 show an example of a method for manufacturing a mini LED display. First, a resin composition of the present invention is applied to a laser-transparent substrate 11 and cured to form a cured product 12, producing a substrate 100 with the cured product (1a). Next, a substrate having a compound semiconductor layer 14 and electrodes 15 on a sapphire substrate 13 is bonded to the cured product 12 with the electrodes 15 facing each other (1b). The sapphire substrate is then thinned and further singulated to produce a laminate 110 in which mini LED elements 16 are laminated on the substrate 100 with the cured product (1c). A temporary adhesive layer 18 is formed on another laser-transparent substrate 17, and the laminate 110 is bonded to the temporary adhesive layer 18 so that the LED elements 16 face each other (1d). Next, a laser beam 19 is irradiated from the substrate 11 side to laser ablate the interface between the substrate 11 and the cured product 12, thereby peeling the substrate 11 (1e). The residue remaining after the laser peeling of the cured product 12 is then washed away with acetone (1f). The mini LED elements 16 on the temporary adhesive layer 18 can be mounted on the circuit board 20-1 facing the circuit board 20-1, and the substrate 17 and the temporary adhesive layer 18 can be removed to form a mini LED display (1g and 1h). Alternatively, the mini LED elements 16 can be transferred onto a substrate 20-2 having catch properties, and then mounted on the circuit board while converting the pitch using a known method such as a pick-and-place method or a stamping method to form a mini LED display (1g and 1h).
[0099] 3 and 4 show another example of a manufacturing method for a mini LED display. First, a resin composition of the present invention is applied to a laser-transparent substrate 21 and cured to form a cured product 22, producing a substrate 200 with the cured product (2a). Next, a substrate having a compound semiconductor layer 24 epitaxially grown on a compound semiconductor substrate 23 and an electrode 25 is bonded to the cured product 22 with the electrode 25 facing each other. The compound semiconductor substrate 23 is then removed with an etching solution 27 to produce a laminate 210 with mini LED elements 26 laminated on the substrate 200 with the cured product (2b and 2c). Next, an inorganic film 28 is formed on the surface of the laminate 210 facing the mini LED elements 26 using chemical vapor deposition, and the laminate 210 is then bonded to a sapphire substrate 29 via the inorganic film 28 (2d). The sapphire substrate 29 is then thinned (2e). Next, laser light 30 is irradiated from the substrate 21 side to laser ablate the interface between the substrate 21 and the cured product 22, thereby peeling off the substrate 21 (2f). Thereafter, residue remaining after laser peeling of the cured product 22 is washed and removed with acetone to obtain a mini LED substrate 220 (2g). The mini LED substrate 220 can be connected to a circuit board to form a mini LED display.
[0100] The present invention will be described below with reference to examples, but the present invention is not limited to these examples.
[0101] [Measurement and Evaluation Methods] (1) Weight Average Molecular Weight The resin obtained in the following synthesis example was dissolved in a developing solution to a concentration of 0.1% by mass to prepare a sample. The obtained sample was measured using a GPC apparatus (Waters Corporation e2695) at a column temperature of 50 ° C. and a flow rate of 0.4 mL / min, and the weight average molecular weight was calculated using a calibration curve of standard polystyrene. The developing solution used was prepared so that lithium chloride and phosphoric acid were each 0.05 mol / L in NMP. The column used was a TSK-GEL α2500 (manufactured by Tosoh) and a TSK-GEL α4000 (manufactured by Tosoh) connected in series. The standard polystyrene used was PL2010-0102 (manufactured by Agilent Technologies, Inc.).
[0102] (2) Dissolution Rate in Acetone The resin compositions obtained in the following Examples and Comparative Examples were applied to a silicon substrate using a spin coater (1H-360S, manufactured by Mikasa Co., Ltd.) and dried at 120°C for 3 minutes using a hot plate (SCW-636, manufactured by Dainippon Screen Co., Ltd.). Thereafter, a heat treatment was carried out using a hot plate at 250°C for 10 minutes to form a cured product on the silicon substrate. The film thickness was measured using an interference film thickness meter (Lambda Ace, manufactured by SCREEN Co., Ltd.), and this was used as the T 1 The film thickness was then measured after immersion in acetone at 25°C for 10 minutes. 2 (nm). (T 1 -T 2 The dissolution rate (nm / min) in acetone was calculated by the following equation:
[0103] (3) Storage Modulus at 200°C The resin compositions obtained in the following Examples and Comparative Examples were applied to the shiny surface of 18 μm-thick electrolytic copper foil using a bar coater and dried at 120°C for 3 minutes using a hot plate (SCW-636, manufactured by Dai-Nippon Screen Co., Ltd.). This was then heat-treated at 250°C for 10 minutes using a hot plate to form a cured product with a film thickness of 10 μm on the copper foil. The copper foil with the cured product was etched with a ferric chloride solution to obtain a single film of the cured product. The resulting single film of the cured product was then cut into a length of 0.5 cm x 3 cm to prepare a strip-shaped sample. This sample was measured using a dynamic viscoelasticity measuring device (DVA-200, manufactured by IT Measurement & Control Co., Ltd.) in tensile mode, at a frequency of 1 Hz, and in the temperature range of 25°C to 250°C, and the storage modulus at 200°C was determined from the obtained temperature-storage modulus curve.
[0104] (4) Glass Transition Temperature The resin compositions obtained in the following Examples and Comparative Examples were applied to the shiny surface of 18 μm-thick electrolytic copper foil using a bar coater and dried for 3 minutes at 120°C using a hot plate (SCW-636, manufactured by Dai-Nippon Screen Co., Ltd.). The coating was then heated for 10 minutes at 250°C using the same hot plate to form a cured product with a film thickness of 10 μm on the copper foil. The copper foil with the cured product was etched with a ferric chloride solution to obtain a single film of cured product. The resulting single film of cured product was then cut into a length of 1.5 cm x 3 cm to prepare a cylindrical sample with a diameter of 2 mm and a length of 1.5 cm. This sample was measured using a thermal analyzer (TMA / SS6600, manufactured by Hitachi High-Tech Science Corporation) in indentation mode over a temperature range of 25°C to 250°C, and the inflection point of the obtained temperature-expansion curve was taken as the glass transition temperature.
[0105] (5) Lamination Ability The resin compositions obtained in the following Examples and Comparative Examples were applied to a 525 μm-thick 4-inch glass substrate using a spin coater (1H-360S, manufactured by Mikasa Co., Ltd.) and dried for 3 minutes at 120°C using a hot plate (SCW-636, manufactured by Dainippon Screen Co., Ltd.). This was then subjected to a heat treatment at 250°C for 10 minutes using a hot plate to form a 10 μm-thick cured product on the 4-inch glass substrate. A 525 μm-thick 4-inch glass substrate was then placed on the cured product-side surface of the glass substrate with the cured product, and the upper and lower plates were pressed together at a pressure of 0.5 MPa for 5 minutes using a heat press set at 200°C. The proportion of the area of the resulting bonded substrate where bonding defects such as lifting or cloudiness occurred to the area of the substrate was calculated, and the lamination ability was evaluated on a 5-point scale according to the following evaluation criteria: C: Fail; B: Poor - A: The area of the portion where poor lamination occurred is less than 0.5% of the area of the substrate. - B: The area of the portion where poor bonding occurred was 0.5% or more and less than 1% of the area of the substrate. B: The area of the portion where poor bonding occurred was 1% or more and less than 3% of the area of the substrate. - : The area of the portion where poor bonding occurred was 3% or more and less than 5% of the area of the substrate. C: The area of the portion where poor bonding occurred was 5% or more of the area of the substrate.
[0106] (6) Durability in Thinning and Heat Treatment Steps The resin compositions obtained in the following Examples and Comparative Examples were applied to a 525 μm-thick 4-inch glass substrate using a spin coater (1H-360S, manufactured by Mikasa Co., Ltd.) and dried for 3 minutes at 120°C using a hot plate (SCW-636, manufactured by Dainippon Screen Co., Ltd.). The resulting coating was then heat-treated for 10 minutes at 250°C using the same hot plate to form a 10 μm-thick cured product on the 4-inch glass substrate. A 525 μm-thick 4-inch glass substrate was then placed on the cured product-side surface of the glass substrate with the cured product, and the upper and lower plates were press-bonded at a pressure of 0.5 MPa for 5 minutes using a heat press machine set to 200°C. The resulting bonded substrates were then polished to a thickness of 5 μm using a grinder (DAG810, manufactured by DISCO Corporation). The polished bonded substrate was heat treated at 200°C for 10 minutes using a hot plate, and after dissipation of heat, the substrate was visually observed to evaluate the presence or absence of cracks after the process. Those that showed cracks were rated as "failed," and those that did not show cracks were rated as "passed."
[0107] (7) Durability in Thinning Process and Heat Treatment Process (250°C) After preparing a bonded substrate in the same manner as in (6) above, the obtained bonded substrate was polished using a grinder (DAG810 manufactured by DISCO Corporation) until each of the two 4-inch glass substrates had a thickness of 5 μm. The polished bonded substrate was heat-treated at 250°C for 10 minutes using a hot plate, and after dissipation, the substrate was visually observed to evaluate the presence or absence of cracks after the process. This evaluation was conducted under stricter conditions than in (6) above, and it is preferable that no cracks occurred even under these conditions.
[0108] (8) Cleanability of Residue After Laser Peeling The resin compositions obtained in the following Examples and Comparative Examples were applied to a 525 μm-thick 4-inch glass substrate using a spin coater (1H-360S, manufactured by Mikasa Co., Ltd.) and dried for 3 minutes at 120°C using a hot plate. The same hot plate was then used to perform a heat treatment at 250°C for 10 minutes to form a 10 μm-thick cured product on the 4-inch glass substrate. A 525 μm-thick 4-inch glass substrate was then placed on the cured product-side surface of the glass substrate with the cured product, and the upper and lower plates were press-bonded together at a pressure of 0.5 MPa for 5 minutes using a heat press set to 200°C. The resulting bonded substrate was irradiated with a 308 nm excimer laser (manufactured by Light Machinery Co., Ltd.) under conditions of an irradiation area of 2 mm × 13 mm, a frequency of 30 Hz, and a scan speed of 19.5 mm / sec, thereby performing full-surface peeling. The two peeled substrates were immersed in acetone at 25°C and washed with ultrasonic waves, and then the cleanability of the residue after laser peeling was evaluated on an 8-point scale according to the following evaluation criteria. E was evaluated as failing, and D or better as passing. A: After 10 minutes of washing, no residue was visually observed on the substrate. A - B: After 20 minutes of cleaning, no residue was visually observed on the substrate. B: After 30 minutes of cleaning, no residue was visually observed on the substrate. - C: After 60 minutes of cleaning, no residue was visually observed on the substrate. C: After 120 minutes of cleaning, no residue was visually observed on the substrate. - A: After 180 minutes of cleaning, no residue was visually observed on the substrate. D: After 240 minutes of cleaning, no residue was visually observed on the substrate. E: After 240 minutes of cleaning, residue was visually observed on the substrate.
[0109] The names and abbreviations of the compounds used in the Examples and Comparative Examples are shown below. <Diamines that provide diamine residue (a1)> APPS1: Modified silicone oil having the structure of formula (1) (average molecular weight: 860, KF8010 manufactured by Shin-Etsu Chemical Co., Ltd.) APPS2: Modified silicone oil having the structure of formula (1) (average molecular weight: 1590, X22-161A manufactured by Shin-Etsu Chemical Co., Ltd.) <Diamines that provide diamine residue (a2)> DDS: 3,3'-diaminodiphenyl sulfone (manufactured by Konishi Chemical Industry Co., Ltd.) <Diamines that provide diamine residue (a5)> m-TB: 2,2'-dimethylbenzidine (manufactured by Wakayama Seika Kogyo Co., Ltd.) Benzidine: 4,4'-diaminobiphenyl (manufactured by Tokyo Chemical Industry Co., Ltd.) <Diamines that provide diamine residues other than diamine residues (a1), (a2), and (a5)> SiDA: tetramethyl-1,3-bis(3-aminopropyl)disiloxane (average molecular weight: 248, LP-7100 manufactured by Shin-Etsu Chemical Co., Ltd.) <Acid dianhydride that provides the acid dianhydride residue (a3)> 6FDA: 4,4'-(hexafluoroisopropylidene)diphthalic dianhydride (manufactured by Merck Ltd.) ODPA: 3,3',4,4'-diphenylethertetracarboxylic dianhydride (manufactured by Toho Chemical Industry Co., Ltd.) BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride (manufactured by Mitsubishi Chemical Corporation) <Acid dianhydride that provides the acid dianhydride residue (a3-1)> 6FDA: 4,4'-(hexafluoroisopropylidene)diphthalic dianhydride (manufactured by Merck Ltd.) <Acid dianhydride that provides the acid dianhydride residue (a3-2)> ODPA: 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride (manufactured by Toho Chemical Industry Co., Ltd.) <Acid dianhydride giving an acid dianhydride residue other than the acid dianhydride residue (a3)> PMDA: pyromellitic dianhydride (manufactured by Daicel Corporation) <Solvent> CHN: cyclohexanone (manufactured by Toyo Gosei Co., Ltd.).
[0110] Example 1 Under a dry nitrogen stream, DDS (16.9 g, 0.068 mol), APPS1 (58.5 g, 0.068 mol), and m-TB (7.2 g, 0.034 mol) were placed in a flask and dissolved in CHN (290.2 g). Subsequently, ODPA (15.8 g, 0.051 mol) and PMDA (26.0 g, 0.12 mol) were added, and the mixture was stirred at 60°C for 1 hour and then at 150°C for 4 hours to obtain a 30% by mass polyimide polymerization solution.
[0111] The above polymerization solution was filtered under pressure using a filter with a retention particle size of 1 μm to obtain a resin composition P1.
[0112] [Examples 2 to 43, Comparative Examples 1 to 15] Resin compositions P2 to P58 were obtained in the same manner as in Synthesis Example 1, except that the types and amounts of diamines and acid dianhydrides were changed as shown in Tables 1 to 12.
[0113]
[0114]
[0115]
[0116]
[0117]
[0118]
[0119]
[0120]
[0121]
[0122]
[0123]
[0124]
[0125] The evaluation results of Examples 1 to 43 and Comparative Examples 1 to 15 are shown in Tables 13 to 24.
[0126]
[0127]
[0128]
[0129]
[0130]
[0131]
[0132]
[0133]
[0134]
[0135]
[0136]
[0137]
[0138] 1a, 2a: Process for producing a substrate with a cured product 1b: Process for bonding a substrate with a cured product to a substrate having a compound semiconductor layer and an electrode 15 1c: Process for producing a laminate in which a mini LED element is laminated on a substrate with a cured product 1d: Process for bonding a laser-transparent substrate to a laminate 1e: Irradiation process 1f, 2g: Process for cleaning and removing residues 1g: Mounting process 1h: Process for removing a substrate and a temporary adhesive layer 2b: Etching process 2c: Process for removing a compound semiconductor substrate 2d: Process for forming an inorganic film and process for bonding a laminate to a sapphire substrate 2e: Process for thinning a sapphire substrate 2f: Laser ablation process 11, 17, 21: Laser-transparent substrate 12, 22: Cured product 13, 29: Sapphire substrate 14, 24: Compound semiconductor layer 15, 25: Electrode 16, 26: Mini LED element 18: Temporary adhesive layer 19, 30: Laser light 20-1: Circuit board 20-2: Substrate having catching properties 23: Compound semiconductor substrate 27: Etching solution 28: Inorganic film 100, 200: Substrate with cured product 110, 210: Laminate 220: Mini LED substrate
Claims
1. A resin composition containing a polyimide-containing resin (A) and a solvent, wherein the resin (A) contains a diamine residue (a1) represented by formula (1) and a diamine residue (a2) represented by formula (2), and the content of diamine residue (a1) is 30.0 mol% or more and less than 50.0 mol% and the content of diamine residue (a2) is 30.0 mol% or more and 70.0 mol% or less, relative to 100.0 mol% of all diamine residues in the resin (A). The content of Si atoms contained in the resin (A) is 12.0 mass% or more and 16.0 mass% or less, relative to 100.0 mass% of the resin (A). In formula (1), R 1 ~R 4 R each independently represents an alkyl group having 1 to 30 carbon atoms, a phenyl group, or a phenoxy group. 5 and R 6 each independently represents an alkylene group or a phenylene group having 1 to 30 carbon atoms, and n represents a range of 5 to 30. * represents the bonding site to the nitrogen atom in the imide group. In formula (2), R 7 ~R 14 each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, a hydroxyl group, or a halogen. * represents the bonding site to the nitrogen atom in the imide group.
2. The resin composition according to claim 1, wherein the molar ratio of the content of the diamine residue (a2) to the content of the diamine residue (a1) in the resin (A) is 0.9 to 1.
6.
3. A resin composition according to claim 1 or 2, wherein the resin (A) contains 50.0 mol % or more and 100.0 mol % or less of the acid dianhydride residue (a3) represented by formula (3), based on 100.0 mol % of all acid anhydride residues. In formula (3), R 15 is a single bond, -C(H 2 )-, -O-, -C(O)-, -C(CH 3 ) 2 -, -S(O 2 ) -, -C(CF 3 ) 2 -, R 16 ~R 21 Each of independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, a hydroxyl group, or a halogen. * represents the bonding site to a carbon atom in the imide group.
4. Resin (A) contains 100.0 mol% of the total acid dianhydride residues (a3) of R in formula (3). 15 -C(CF 3 ) 2 The resin composition according to claim 3, comprising 20.0 mol % or more and less than 80.0 mol % of an acid dianhydride residue (a3-1) represented by the formula:
5. The ratio of R in formula (3) to the content of the acid dianhydride residue (a3-1) in the resin (A) 15 The resin composition according to claim 4, wherein the molar ratio of the content of the acid dianhydride residue (a3-2) in which is -O- is 0.97 to 1.
02.
6. The resin composition according to claim 1 or 2, wherein the resin (A) further contains a diamine residue (a5) represented by formula (5), and the content of the diamine residue (a5) in 100.0 mol% of all diamine residues in the resin (A) is 10.0 mol% or more and 30.0 mol% or less. In formula (5), R 22 ~R 29 each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, a hydroxyl group, or a halogen atom. * represents a bonding site to a carbon atom in the imide group.
7. The resin composition according to claim 6, wherein the diamine residue (a5) is a diamine residue having a structure represented by formula (6). In formula (6), * represents the bonding site to the carbon atom in the imide group.
8. The resin composition according to claim 1 or 2, wherein the weight average molecular weight of the resin (A) is 10,000 or more and 30,000 or less.
9. A cured product derived from the resin composition according to claim 1 or 2.
10. The cured product according to claim 9, having a dissolution rate in acetone of 100 nm / min or more and less than 10,000 nm / min.
11. The cured product according to claim 9, having a storage modulus at 200°C of 0.5 MPa or more and less than 5.0 MPa.
12. A substrate having the cured product according to claim 9 formed on a supporting substrate.
13. A laminate comprising a substrate with the cured product according to claim 12 and a semiconductor element laminated thereon.
14. A method for manufacturing a semiconductor device, which uses the resin composition according to claim 1 or 2.
15. A method for manufacturing a semiconductor device, using the cured product according to claim 9.
16. A method for manufacturing a semiconductor device, using a substrate with the cured product according to claim 12.
17. A method for manufacturing a semiconductor device, using the laminate according to claim 13.
Citation Information
Patent Citations
High-temperature-resistant high-solubility polyimide core strip adhesive and preparation method thereof
CN115305046A
Heat-resistant resin adhesive
JP1993025453A
New polyimide and its production
JP1997067438A
Polyamic acid copolymer, polyimide copolymer and heat-resistant adhesive
JP1999222522A
Solvent-soluble polyimide copolymer
JP2005120176A
Cited By
Resin composition, cured film, laminate, electronic component, and method for producing electronic component
WO2026211135A1