Positive photosensitive pigment composition, cured product, and organic el display device

The positive photosensitive pigment composition, featuring dioxazine or perylene pigments and specific additives, addresses residue and uniformity issues in organic EL display devices, enhancing light-shielding and brightness by forming well-defined pixel division layers with improved halftone processing.

WO2024204339A1PCT designated stage expired Publication Date: 2024-10-03TORAY INDUSTRIES INC

Patent Information

Application Number
PCT/JP2024/012241
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing positive photosensitive pigment compositions for organic electroluminescence (EL) display devices face issues with residue generation, in-plane uniformity, and insufficient light-shielding properties when forming pixel division layers, which affect the brightness and reflectivity of organic EL display devices.

Method used

A positive photosensitive pigment composition comprising a dioxazine or perylene pigment with a benzimidazole skeleton, an alkali-soluble resin, a phenolic hydroxyl group-containing compound, a photoacid generator, and organic dye particles, optimized to suppress residue formation and enhance light-shielding properties while maintaining high exposure sensitivity.

Benefits of technology

The composition effectively suppresses residue generation, achieves high in-plane uniformity, and provides excellent light-shielding properties, improving the brightness and reflectivity of organic EL display devices by forming pixel division layers with steps through halftone processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012241_03102024_PF_FP_ABST
    Figure JP2024012241_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing a positive photosensitive pigment composition which ensures no residue in a pattern opening part and with which it is possible to collectively form a pixel division layer and a spacer layer having a high level of light shielding. The present invention is a positive photosensitive pigment composition containing: a pigment (a) which is a dioxazine pigment and / or a perylene pigment having a benzimidazole skeleton; an alkali-soluble resin (b); a compound (c) having a phenolic hydroxyl group and a molecular weight of at most 1,000; a photoacid generator (d); and a solvent (e), wherein the compound (c) contains a compound (c1) having a C5-C20 alkyl group.
Need to check novelty before this filing date? Find Prior Art

Description

Positive photosensitive pigment composition, cured product, and organic EL display device

[0001] The present invention relates to a positive photosensitive pigment composition, a cured product, and an organic EL display device.

[0002] In recent years, products equipped with flexible organic electroluminescence (EL) display devices have been developed. By eliminating the thick polarizing plate that was previously placed on the front of the panel, not only is the panel more flexible, but brightness loss is also eliminated, and this is expected to improve the lifespan of the light-emitting pixels. The light-emitting elements of organic EL display devices are arranged with a pattern that functions as an insulating layer, known as a pixel dividing layer or pixel defining layer, to separate each light-emitting pixel. To replace the function of the polarizing plate, it is necessary to provide a function to suppress reflection of external light, such as sunlight, and technology to provide light-blocking properties to the pixel dividing layer has attracted attention.

[0003] Incidentally, in order to improve yield during panel production, when forming a light-emitting layer in the openings of the pixel division layer by patterned vapor deposition, a technology (halftone processing) is known in which a pixel division layer having a stepped shape is formed in one go by a photolithography method including an exposure step of irradiating exposure light containing at least near-ultraviolet light through a halftone exposure mask having fully transparent portions, semi-transparent portions, and opaque portions in its plane, in order to reduce the contact area between the vapor deposition mask and the pixel division layer. Halftone processing is useful because it can significantly reduce manufacturing process costs compared to two-layer processing, which forms a thin film portion and then laminates a thick film portion.

[0004] As a material for collectively forming a black pixel division layer having a stepped shape by halftone processing, a negative or positive photosensitive composition containing an organic pigment as a black material has been proposed because of its excellent insulating properties and heat resistance. For example, a negative photosensitive pigment composition is disclosed in Patent Document 1, and positive photosensitive pigment compositions containing an organic pigment are disclosed in Patent Documents 2 and 3.

[0005] International Publication No. 2018 / 180592 International Publication No. 2022 / 270182 Patent No. 7120022

[0006] However, when a black pixel division layer having a step is formed in one step using the negative photosensitive pigment composition disclosed in Patent Document 1, the halftone processability is insufficient, resulting in low in-plane uniformity of the aperture width, particularly in high-definition panels designed with a small aperture width, resulting in brightness unevenness in the organic EL display device. On the other hand, when the positive photosensitive pigment composition disclosed in Patent Document 2 is used, the in-plane uniformity of the aperture width is high and a pixel division layer having a step can be formed with high exposure sensitivity, but there is a problem that pigment-derived residue is generated on the surface of the aperture, resulting in dark spots in at least some of the light-emitting pixels of the organic EL display device. Furthermore, when the positive photosensitive pigment composition disclosed in Patent Document 3 is used, pigment-derived residue on the aperture is suppressed and the occurrence of dark spots is suppressed, but the light-blocking properties of the pixel division layer are low and the effect of suppressing the above-mentioned external light reflection is insufficient. For these reasons, there has been a strong demand for a photosensitive composition that can suppress residue on the surface of the aperture, have high light-blocking properties, and form a pixel division layer having a step.

[0007] The present inventors have conducted extensive research and found that a photosensitive composition having the following configuration can solve the above-mentioned problems. [1] A positive photosensitive pigment composition comprising a pigment (a) that is a dioxazine pigment and / or a perylene pigment having a benzimidazole skeleton, an alkali-soluble resin (b), a compound (c) having a phenolic hydroxyl group and a molecular weight of 1,000 or less, a photoacid generator (d), and a solvent (e), wherein compound (c) contains a compound (c1) having an alkyl group having 5 to 20 carbon atoms. [2] The positive photosensitive pigment composition according to [1], further comprising organic dye particles (f) having a sulfo group. [3] The positive photosensitive pigment composition according to [1] or [2], wherein the content of pigment (a) is 10 to 30 mass% based on 100 mass% of the solid content of the positive photosensitive pigment composition. [4] The positive photosensitive pigment composition according to any one of [1] to [3], wherein compound (c1) contains a compound represented by formula (1).

[0008]

[0009] In formula (1), R 1 represents —NH— or an oxygen atom.2 represents an alkyl group having 5 to 20 carbon atoms. 3 , R 4 , R 5 , R 6 and R 7 each independently represents a hydrogen atom, an alkyl group, or a hydroxyl group. 3 , R 4 , R 5 , R 6 and R 7 wherein the total number of hydroxyl groups is 1 to 3. [5] The positive photosensitive pigment composition according to any one of [1] to [4], wherein compound (c1) contains a compound having an alkyl group having 12 to 18 carbon atoms. [6] The positive photosensitive pigment composition according to any one of [1] to [5], wherein compound (c) contains a compound (c2) that does not have an alkyl group having 5 to 20 carbon atoms and has an aryl group substituted with three or more phenolic hydroxyl groups. [7] The positive photosensitive pigment composition according to [6], wherein compound (c2) is a compound represented by formula (40):

[0010]

[0011] In formula (40), n 24 is 3 to 6. [8] The positive photosensitive pigment composition according to [6], wherein the content of compound (c1) in compound (c) is 15 to 70 mass % and the content of compound (c2) in compound (c) is 30 to 85 mass %. [9] The positive photosensitive pigment composition according to [7], wherein the ratio mc1 / mc2 of the content (by mass) of compound (c1) to the content (by mass) mc2 of compound (c2) is 0.3 or more and less than 1.0.

[10] A cured product derived from the positive photosensitive pigment composition according to any one of [1] to [9].

[11] An organic EL display device comprising the cured product according to

[10] .

[0012] The positive photosensitive pigment composition of the present invention suppresses the generation of residues on the surface of the openings, has high light-shielding properties, and can form pixel division layers having steps in one step by halftone processing.

[0013] 1 is a cross-sectional view of a TFT substrate in an organic EL display device that is a specific example of an embodiment of the present invention, and shows a manufacturing process of an organic EL display device including a step of forming a pixel dividing layer in all examples and comparative examples.

[0014] The present invention will be described in detail below. In the present invention, the term "solid content" refers to the composition excluding the solvent.

[0015] The positive photosensitive pigment composition of the present invention contains a pigment (a), an alkali-soluble resin (b), a compound having a phenolic hydroxyl group and a molecular weight of 1,000 or less (c), a photoacid generator (d), and a solvent (e).

[0016] <Pigment (a)> Pigment (a) is a dioxazine pigment and / or a perylene pigment having a benzimidazole skeleton. Pigment (a) provides light-blocking properties to the pixel division layer obtained in the end. Compared with the minimum transmittance in the wavelength range of 500 to 600 nm, the maximum transmittance in the wavelength range of 300 to 450 nm is preferably higher, resulting in excellent optical density. Furthermore, it is easy for exposure light containing at least light in the wavelength range of 300 to 450 nm to penetrate deep into the film, resulting in high exposure sensitivity in halftone processing.

[0017] Preferred examples of perylene pigments having a benzimidazole skeleton include compounds represented by formula (2) and / or compounds represented by formula (3).

[0018]

[0019]

[0020] In formula (2) and formula (3), R 8 ~R 15 R each independently represents a hydrogen atom, a fluorine atom, a bromine atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms. 16 ~R 23 each independently represents a hydrogen atom, a fluorine atom, a bromine atom or a hydroxyl group.

[0021] An example of a commercially available perylene pigment having a benzimidazole skeleton is "Spectrasense" (registered trademark) Black K0087 (manufactured by BASF), which is a mixture of cis and trans isomers of 3,4,9,10-perylenetetracarboxylic acid bisbenzimidazole.

[0022] Preferred examples of dioxazine pigments include dioxazine pigments having a carboxylic acid amide bond and / or a carboxylic acid ester bond in the molecule. Having a carboxylic acid amide bond means having a group represented by -CONH-. Therefore, this does not include sulfonamide bonds or phosphate amide bonds. Having a carboxylic acid ester bond means having a group represented by -COO-. Therefore, this does not include sulfonyl ester bonds or phosphate ester bonds. Here, the term "dioxazine pigment" refers to an organic pigment containing a compound that has a triphenodioxazine skeleton in the molecule and does not have a sulfo group. Note that a mixture of a compound that has a triphenodioxazine skeleton but does not have a sulfo group and an organic dye that has a sulfo group, or a mixed crystal, is defined as a mixture of a dioxazine pigment and organic dye particles (f). The term "triphenodioxazine skeleton" refers to a skeleton represented by formula (4):

[0023]

[0024] Specific examples of dioxazine pigments include triphenodioxazine pigments represented by formulas (5) to (16). The dioxazine pigments may be a mixture or mixed crystal of two or more kinds.

[0025]

[0026]

[0027]

[0028]

[0029]

[0030]

[0031]

[0032]

[0033]

[0034]

[0035]

[0036]

[0037] The method for synthesizing the dioxazine pigment is not particularly limited, but for example, the method described in French Patent Application Publication No. 1269107 can be referred to.

[0038] The average primary particle diameter of pigment (a) is preferably 10 nm or more, more preferably 20 nm or more, in order to improve halftone processability. From the same viewpoint, it is preferably 100 nm or less, more preferably 80 nm or less. The average primary particle diameter here refers to the number-average primary particle diameter calculated by a particle size measurement method using an image analysis particle size distribution analyzer. A transmission electron microscope (TEM) can be used to capture images, and the average primary particle diameter can be calculated by analyzing 50 primary particles randomly selected from an image of 100 or more primary particles of pigment (a) captured at a magnification of 50,000x. If pigment (a) is not spherical, the primary particle diameter (nm) is determined by rounding the average major axis of the particles to one decimal place. Furthermore, the maximum major axis of the 50 primary particles selected from the same TEM image used to calculate the average primary particle diameter is defined as the maximum primary particle diameter. The maximum primary particle size of the pigment (a) is preferably 200 nm or less, more preferably 150 nm or less, in order to improve halftone processability. For image analysis, image analysis particle size distribution software Mac-View (manufactured by Mountech Co., Ltd.; JIS 8827-1 compliant; particle size analysis - image analysis method) can be used.

[0039] The content of the pigment (a) is preferably 10% by mass or more, based on 100% by mass of the solid content of the positive photosensitive pigment composition, in order to improve the light-shielding property of the pixel division layer, and is preferably 30% by mass or less, more preferably 20% by mass or less, in order to improve halftone processability.

[0040] <Alkali-Soluble Resin (b)> The positive photosensitive pigment composition of the present invention contains an alkali-soluble resin (b). The alkali-soluble resin (b) refers to a dissolution rate of 50 nm or more per minute, determined from the decrease in film thickness when a solution of the resin dissolved in γ-butyrolactone is applied to a silicon wafer and prebaked at 120°C for 4 minutes to form a prebaked film having a film thickness of 10 μm±0.5 μm, the prebaked film is then immersed in a 2.38 mass% aqueous solution of tetramethylammonium hydroxide at 23±1°C for 1 minute, and then rinsed with pure water. The term "resin" as used herein refers to a compound having a polymer chain with five or more repeating units and a weight-average molecular weight (Mw) of 1,000 or more.

[0041] The alkali-soluble resin (b) has alkali solubility and therefore has hydroxyl groups and / or acidic groups in the structural units of the resin and / or at the ends of its main chain. The acidic groups may include, for example, carboxyl groups, phenolic hydroxyl groups, sulfonic acid groups, etc.

[0042] The alkali-soluble resin (b) may include, but is not limited to, known compounds such as polyimide, polyimide precursor, polybenzoxazole, polybenzoxazole precursor, polyamideimide, polyamideimide precursor, polyamide, polymer of radically polymerizable monomer having an acidic group, siloxane resin, cardo resin, and phenolic resin. The positive-tone photosensitive pigment composition of the present invention may contain two or more of these resins. Among these alkali-soluble resins (b), the alkali-soluble resin (b) preferably contains one or more selected from the group consisting of polyimide, polyimide precursor, polybenzoxazole, polybenzoxazole precursor, polyamideimide, polyamideimide precursor, and copolymers thereof, because of its high development adhesion, excellent heat resistance, and low outgassing at high temperatures, resulting in high long-term reliability when the cured product is used in an organic EL display device. Polyimide, polyimide precursor, polybenzoxazole precursor, or copolymers thereof is more preferred. Furthermore, from the viewpoint of further improving sensitivity, the alkali-soluble resin (b) preferably contains a polyimide precursor or polybenzoxazole precursor. Here, the polyimide precursor refers to a resin that can be converted into a polyimide by heat treatment or chemical treatment, such as polyamic acid, polyamic acid ester, etc. The polybenzoxazole precursor refers to a resin that can be converted into a polybenzoxazole by heat treatment or chemical treatment, such as polyhydroxyamide, etc.

[0043] The polyimide precursor and polybenzoxazole precursor described above have a structural unit represented by the following formula (17), and the polyimide has a structural unit represented by the following formula (18). Two or more of these may be contained, or a resin in which the structural unit represented by formula (17) and the structural unit represented by formula (18) are copolymerized may be contained.

[0044]

[0045] In formula (17), X represents a divalent to octavalent organic group having 4 to 40 carbon atoms, and Y represents a divalent to elevenvalent organic group having 6 to 40 carbon atoms. 24 and R 26R each independently represents a hydroxyl group or a sulfonic acid group. 25 and R 27 each independently represents a hydrogen atom or a monovalent hydrocarbon group having 1 to 20 carbon atoms. t, u, and w represent integers of 0 to 3, and v represents an integer of 0 to 6. However, when the structural unit represented by formula (3) represents a structural unit of a polyimide precursor, u≧2; when the structural unit represented by formula (3) represents a structural unit of a polybenzoxazole precursor, v≧2; and when a plurality of R 26 At least two of these are hydroxyl groups.

[0046]

[0047] In formula (18), E represents a tetravalent to decavalent organic group having 4 to 40 carbon atoms, and G represents a divalent to octavalent organic group having 6 to 40 carbon atoms. 28 and R 29 each independently represents a carboxy group, a sulfonic acid group, or a hydroxyl group, and x and y each independently represent an integer of 0 to 6, provided that x+y>0.

[0048] In the above formula (17), X(R 24 ) t (COOR 25 ) u represents an acid residue. X is a divalent to octavalent organic group having 4 to 40 carbon atoms, and is preferably a divalent to octavalent organic group containing an aromatic ring or a cycloaliphatic group.

[0049] Examples of acid residues include residues of dicarboxylic acids such as terephthalic acid, isophthalic acid, diphenyl ether dicarboxylic acid, bis(carboxyphenyl)hexafluoropropane, biphenyl dicarboxylic acid, benzophenone dicarboxylic acid, and triphenyl dicarboxylic acid; residues of tricarboxylic acids such as trimellitic acid, trimesic acid, diphenyl ether tricarboxylic acid, and biphenyl tricarboxylic acid; residues of pyromellitic acid, 3,3',4,4'-biphenyl tetracarboxylic acid, 2,3,3',4'-biphenyl tetracarboxylic acid, 2,2',3,3'-biphenyl tetracarboxylic acid, 3,3',4,4'-benzophenone tetracarboxylic acid, 2,2',3,3'-benzophenone tetracarboxylic acid, 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane, and 2,2-bis(2,3-dicarboxyphenyl)hexafluoropropane. Examples of the structural unit include residues of tetracarboxylic acids such as 1,1-bis(3,4-dicarboxyphenyl)hexafluoropropane, 1,1-bis(3,4-dicarboxyphenyl)ethane, 1,1-bis(2,3-dicarboxyphenyl)ethane, bis(3,4-dicarboxyphenyl)methane, bis(2,3-dicarboxyphenyl)methane, bis(3,4-dicarboxyphenyl)ether, 1,2,5,6-naphthalenetetracarboxylic acid, 2,3,6,7-naphthalenetetracarboxylic acid, 2,3,5,6-pyridinetetracarboxylic acid, 3,4,9,10-perylenetetracarboxylic acid, and aromatic tetracarboxylic acids having the structure shown in the following formula: aliphatic tetracarboxylic acids such as butanetetracarboxylic acid, and aliphatic tetracarboxylic acids containing a cyclic aliphatic group such as 1,2,3,4-cyclopentanetetracarboxylic acid. The polyimide precursor and polybenzoxazole precursor having the structural unit represented by formula (17) may have two or more of these residues.

[0050]

[0051] In the above formula, R 30 is an oxygen atom, C(CF 3 ) 2 or C(CH 3 ) 2 Represents R 31 and R 32each independently represents a hydrogen atom or a hydroxyl group. In the case of a residue of a tricarboxylic acid or a tetracarboxylic acid, one or two carboxy groups are (COOR 25 ) is equivalent to

[0052] In the above formula (18), E(R 28 ) x represents a residue of an acid dianhydride. E is a tetravalent to decavalent organic group having 4 to 40 carbon atoms, and is preferably an organic group containing an aromatic ring or a cycloaliphatic group.

[0053] Examples of the residue of the acid dianhydride include pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 2,2',3,3'-benzophenonetetracarboxylic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 2,2-bis(2,3-dicarboxyphenyl)propane dianhydride, 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, bis(3,4-dicarboxyphenyl)methane dianhydride, bis(2,3-dicarboxyphenyl)methane dianhydride, bis(3,4-dicarboxyphenyl)acetonitrile Examples of the structural unit include aromatic tetracarboxylic dianhydrides such as tetracarboxylic acid dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, 9,9-bis{4-(3,4-dicarboxyphenoxy)phenyl}fluorene dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 2,3,5,6-pyridinetetracarboxylic dianhydride, 3,4,9,10-perylenetetracarboxylic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride, and acid dianhydrides having the structure shown in the following formula: aliphatic tetracarboxylic dianhydrides such as butanetetracarboxylic dianhydride, and aliphatic tetracarboxylic dianhydrides containing a cyclic aliphatic group such as 1,2,3,4-cyclopentanetetracarboxylic dianhydride. The polyimide having the structural unit represented by formula (18) may have two or more of these residues.

[0054]

[0055] In the above formula, R 30 is an oxygen atom, C(CF 3 ) 2 or C(CH 3 ) 2 Represents R 31 and R 32 each independently represents a hydrogen atom or a hydroxyl group.

[0056] Y(R 26 ) v (COOR 27 ) w and G(R 29 ) y represents a residue of a diamine. Y is a di- to eleven-valent organic group having 6 to 40 carbon atoms, and is preferably a di- to eleven-valent organic group containing an aromatic ring or a cycloaliphatic group. G is a di- to octa-valent organic group having 6 to 40 carbon atoms, and is preferably a di- to octa-valent organic group containing an aromatic ring or a cycloaliphatic group.

[0057] Specific examples of the diamine residue include 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 1,4-bis(4-aminophenoxy)benzene, benzidine, m-phenylenediamine, p-phenylenediamine, 1,5-naphthalenediamine, 2,6-naphthalenediamine, bis(4-aminophenoxy)biphenyl, bis{4-(4-aminophenoxy)phenyl}ether, 1,4-bis(4-aminophenoxy)benzene, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-diethyl-4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminobiphenyl, and 3,3'-diethyl-4,4'-diaminobiphenyl. The amine may contain residues of aromatic diamines such as phenyl, 2,2',3,3'-tetramethyl-4,4'-diaminobiphenyl, 3,3',4,4'-tetramethyl-4,4'-diaminobiphenyl, 2,2'-di(trifluoromethyl)-4,4'-diaminobiphenyl, 9,9-bis(4-aminophenyl)fluorene, 2,2'-bis(trifluoromethyl)-5,5'-dihydroxybenzidine, 3,5-diaminobenzoic acid, 3,4-diaminobenzoic acid, 2,5-diaminobenzoic acid, and compounds in which at least a portion of the hydrogen atoms in the aromatic rings of these are substituted with alkyl groups or halogen atoms; residues of aliphatic diamines containing cyclic aliphatic groups such as cyclohexyldiamine and methylenebiscyclohexylamine; and residues of diamines having a structure represented by the following formula: The polyimide precursor and polybenzoxazole precursor having the structural unit represented by formula (17) and the polyimide having the structural unit represented by formula (18) may have two or more types of these residues.

[0058]

[0059] In the above formula, R 30 is an oxygen atom, C(CF 3 ) 2 or C(CH 3 ) 2 Represents R 31 ~R 34 each independently represents a hydrogen atom or a hydroxyl group.

[0060] The polyimide precursor and polybenzoxazole precursor having a structural unit represented by formula (17), the polyimide having a structural unit represented by formula (18), and the resin obtained by copolymerizing the structural unit represented by formula (17) and the structural unit represented by formula (18) may have their ends capped with a known monoamine, acid anhydride, acid chloride, monocarboxylic acid, or active ester compound having an acidic group.

[0061] The polyimide, polyimide precursor, polybenzoxazole precursor, or copolymer thereof preferably has 5 to 100,000 structural units represented by formula (17) or formula (18). Furthermore, in addition to the structural units represented by formula (17) or formula (18), other structural units may be contained. In this case, it is preferable that the structural units represented by formula (17) or formula (18) account for 50 mol % or more of 100 mol % of all structural units.

[0062] The alkali-soluble resin (b) may be synthesized by a known method. Examples of a method for producing a polyamic acid, which is a polyimide precursor, include a method of reacting a tetracarboxylic dianhydride with a diamine compound in a solvent at low temperature.

[0063]

[0013] In addition to the aforementioned method of reacting a polyamic acid with an esterifying agent, other methods for producing a polyamic acid ester, which is also a polyimide precursor, include a method of obtaining a diester from a tetracarboxylic dianhydride and an alcohol, followed by reacting the diester with an amine in a solvent in the presence of a condensing agent, and a method of obtaining a diester from a tetracarboxylic dianhydride and an alcohol, followed by converting the remaining dicarboxylic acid into an acid chloride and reacting the resulting diester with an amine in a solvent. From the viewpoint of ease of synthesis, it is preferable to include a step of reacting a polyamic acid with an esterifying agent. The esterifying agent is not particularly limited, and known methods can be used, but N,N-dimethylformamide dialkyl acetal is preferred because the resulting resin can be easily purified.

[0064] Examples of methods for producing polyhydroxyamide, a polybenzoxazole precursor, include a method of condensing a bisaminophenol compound with a dicarboxylic acid in a solvent. Specifically, examples include a method of reacting a dehydration condensation agent such as dicyclohexylcarbodiimide (DCC) with an acid and then adding a bisaminophenol compound. Examples include a method of adding a dicarboxylic acid dichloride solution dropwise to a solution of a bisaminophenol compound to which a tertiary amine such as pyridine has been added. Examples of methods for producing polyimide include a method of dehydrating and ring-closing the polyamic acid or polyamic acid ester obtained by the above-mentioned method in a solvent. Examples of methods for dehydration and ring-closing include chemical treatment with an acid or base, and heat treatment.

[0065] Examples of methods for producing polybenzoxazole include a method in which the polyhydroxyamide obtained by the above-mentioned method is subjected to dehydration and ring-closure in a solvent, such as a chemical treatment with an acid or a base, or a heat treatment.

[0066] Examples of the polyamide-imide precursor include a polymer of a tricarboxylic acid, a corresponding tricarboxylic acid anhydride, a tricarboxylic acid anhydride halide, and a diamine compound, and a polymer of trimellitic acid chloride anhydride and an aromatic diamine compound is preferred. Examples of a method for producing the polyamide-imide precursor include a method of reacting a tricarboxylic acid, a corresponding tricarboxylic acid anhydride, a tricarboxylic acid anhydride halide, or the like with a diamine compound in a solvent at low temperature.

[0067] Examples of methods for producing polyamideimide include a method of reacting trimellitic anhydride with an aromatic diisocyanate in a solvent, and a method of dehydrating and cyclizing the polyamideimide precursor obtained by the above method in a solvent. Examples of methods for dehydrating and cyclizing include chemical treatment with an acid or a base, and heat treatment.

[0068] Examples of polymers of radically polymerizable monomers having an acidic group include acrylic resins and polyhydroxystyrene resins. Examples of radically polymerizable monomers having an acidic group include o-hydroxystyrene, m-hydroxystyrene, and p-hydroxystyrene, as well as alkyl- and alkoxy-substituted derivatives thereof, methacrylic acid and acrylic acid, and their α-position haloalkyl-, alkoxy-, halogen-, nitro-, and cyano-substituted derivatives. Among these, o-hydroxystyrene, m-hydroxystyrene, and p-hydroxystyrene, as well as their alkyl- and alkoxy-substituted derivatives, are particularly preferred in terms of sensitivity and resolution during patterning, film remaining rate after development, heat distortion resistance, solvent resistance, adhesion to the base, solution storage stability, and the like. These may be used alone or in combination of two or more.

[0069] Other examples of radical polymerizable monomers having an acidic group include styrene, alkyl, alkoxy, halogen, haloalkyl, nitro, cyano, amide, and ester substitutions at the α-, o-, m-, or p-position of styrene, diolefins such as butadiene and isoprene, and esterified products of methacrylic acid or acrylic acid. These may be used alone or in combination of two or more.

[0070] Cardo resins include resins having a cardo structure, i.e., a backbone structure in which two rings are bonded to a quaternary carbon atom that constitutes a ring. A typical cardo structure is a fluorene ring bonded to a benzene ring.

[0071] Specific examples of a skeletal structure in which two cyclic structures are bonded to a quaternary carbon atom constituting a cyclic structure include a fluorene skeleton, a bisphenolfluorene skeleton, a bisaminophenylfluorene skeleton, a fluorene skeleton having an epoxy group, and a fluorene skeleton having an acrylic group.

[0072] Cardo resins are formed by polymerization of the cardo structure, which is a backbone formed by the reaction between the functional groups attached to the backbone. Cardo resins have a structure (cardo structure) in which the main chain and bulky side chains are connected by a single element, and have a cyclic structure oriented almost perpendicular to the main chain.

[0073] Specific examples of monomers having a cardo structure include known monomers such as bis(glycidyloxyphenyl)fluorene epoxy resins, cardo structure-containing bisphenols such as 9,9-bis(4-hydroxyphenyl)fluorene and 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 9,9-bis(cyanoalkyl)fluorenes such as 9,9-bis(cyanomethyl)fluorene, and 9,9-bis(aminoalkyl)fluorenes such as 9,9-bis(3-aminopropyl)fluorene.

[0074] A cardo resin is a polymer obtained by polymerizing a monomer having a cardo structure, but it may also be a copolymer with other copolymerizable monomers.

[0075] The phenolic resins include well-known ones such as novolak phenolic resins and resol phenolic resins, which can be obtained by polycondensing various phenols alone or a mixture of several of them with aldehydes such as formalin.

[0076] Examples of phenols constituting novolak phenolic resins and resol phenolic resins include phenol, p-cresol, m-cresol, o-cresol, 2,3-dimethylphenol, 2,4-dimethylphenol, 2,5-dimethylphenol, 2,6-dimethylphenol, 3,4-dimethylphenol, 3,5-dimethylphenol, 2,3,4-trimethylphenol, 2,3,5-trimethylphenol, 3,4,5-trimethylphenol, 2,4,5-trimethylphenol, methylenebisphenol, and methylenebisp-cresol. phenol, resorcinol, catechol, 2-methylresorcinol, 4-methylresorcinol, o-chlorophenol, m-chlorophenol, p-chlorophenol, 2,3-dichlorophenol, m-methoxyphenol, p-methoxyphenol, p-butoxyphenol, o-ethylphenol, m-ethylphenol, p-ethylphenol, 2,3-diethylphenol, 2,5-diethylphenol, p-isopropylphenol, α-naphthol, β-naphthol, and the like, which can be used alone or as a mixture of two or more thereof.

[0077] In addition to formalin, examples of aldehydes include paraformaldehyde, acetaldehyde, benzaldehyde, hydroxybenzaldehyde, and chloroacetaldehyde, which can be used alone or in combination.

[0078] Examples of polysiloxanes include known polysiloxanes obtained by hydrolyzing and dehydrating condensation of one or more organosilanes selected from tetrafunctional organosilanes, trifunctional organosilanes, difunctional organosilanes, and monofunctional organosilanes.

[0079] Specific examples of organosilanes include tetrafunctional silanes such as tetramethoxysilane, tetraethoxysilane, tetraacetoxysilane, and tetraphenoxysilane, methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, p-hydroxyphenyltrimethoxysilane, and 1-(p-hydroxyphenyl)trimethoxysilane. (diphenyl)ethyltrimethoxysilane, 2-(p-hydroxyphenyl)ethyltrimethoxysilane, 4-hydroxy-5-(p-hydroxyphenylcarbonyloxy)pentyltrimethoxysilane, trifluoromethyltrimethoxysilane, trifluoromethyltriethoxysilane, 3,3,3-trifluoropropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,trifunctional silanes such as (4-epoxycyclohexyl)ethyltriethoxysilane, (3-ethyl-3-oxetanyl)methoxy]propyltrimethoxysilane, (3-ethyl-3-oxetanyl)methoxy]propyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-trimethoxysilylpropylsuccinic acid, 1-naphthyltrimethoxysilane, 1-naphthyltriethoxysilane, 1-naphthyltri-n-propoxysilane, and 2-naphthyltrimethoxysilane; dimethyldimethoxysilane; dimethyldiethoxysilane; Examples of suitable organosilanes include bifunctional silanes such as silane, dimethyldiacetoxysilane, di-n-butyldimethoxysilane, diphenyldimethoxysilane, (3-glycidoxypropyl)methyldimethoxysilane, (3-glycidoxypropyl)methyldiethoxysilane, di(1-naphthyl)dimethoxysilane, and di(1-naphthyl)diethoxysilane; and monofunctional silanes such as trimethylmethoxysilane, tri-n-butylethoxysilane, (3-glycidoxypropyl)dimethylmethoxysilane, and (3-glycidoxypropyl)dimethylethoxysilane. Two or more of these organosilanes may be used. Furthermore, silicate compounds such as Methyl Silicate 51 manufactured by Fuso Chemical Co., Ltd. and M Silicate 51 manufactured by Tama Chemical Co., Ltd. may also be copolymerized.

[0080] Polysiloxanes are synthesized by hydrolysis and partial condensation of monomers such as organosilanes. Here, partial condensation refers to leaving some Si-OH groups in the resulting polysiloxane, rather than condensing all of the Si-OH groups in the hydrolyzate. Conventional methods can be used for hydrolysis and partial condensation. For example, a solvent, water, and optionally a catalyst are added to an organosilane mixture, followed by heating and stirring at 50 to 150°C for approximately 0.5 to 100 hours. During stirring, hydrolysis by-products (alcohols such as methanol) and condensation by-products (water) may be removed by distillation, if necessary.

[0081] The catalyst is not particularly limited, but an acid catalyst or a base catalyst is preferably used. Specific examples of the acid catalyst include hydrochloric acid, nitric acid, sulfuric acid, hydrofluoric acid, phosphoric acid, acetic acid, trifluoroacetic acid, formic acid, polycarboxylic acids or their anhydrides, and ion exchange resins. Specific examples of the base catalyst include triethylamine, tripropylamine, tributylamine, tripentylamine, trihexylamine, triheptylamine, trioctylamine, diethylamine, triethanolamine, diethanolamine, sodium hydroxide, potassium hydroxide, alkoxysilanes having an amino group, and ion exchange resins.

[0082] The solvent used in the production of the alkali-soluble resin (b) is not particularly limited, and examples thereof include alkylene glycol monoalkyl ethers such as ethylene glycol monomethyl ether and propylene glycol monomethyl ether, alkyl acetates such as propyl acetate, butyl acetate and isobutyl acetate, ketones such as methyl isobutyl ketone and methyl propyl ketone, alcohols such as butyl alcohol and isobutyl alcohol, ethyl lactate, butyl lactate, dipropylene glycol dimethyl ether, diethylene glycol dimethyl ether, diethylene glycol ethyl methyl ether, diethylene glycol diethyl ether, 3-methoxybutyl acetate, ethylene glycol monoethyl ether acetate, gamma butyrolactone, N-methyl-2-pyrrolidone, diacetone alcohol, N-cyclohexyl-2-pyrrolidone, N,N-dimethylformamide ... It may contain methyl acetamide, dimethyl sulfoxide, propylene glycol monomethyl ether acetate, N,N-dimethylisobutyric acid amide, 3-methoxy-N,N-dimethylpropionamide, 3-butoxy-N,N-dimethylpropionamide, 1,3-dimethyl-2-imidazolidinone, N,N-dimethylpropylene urea, delta valerolactone, 2-phenoxyethanol, 2-pyrrolidone, 2-methyl-1,3-propanediol, diethylene glycol butyl ether, triacetin, butyl benzoate, cyclohexylbenzene, bicyclohexyl, o-nitroanisole, diethylene glycol monobutyl ether, triethylene glycol monomethyl ether, N-(2-hydroxyethyl)-2-pyrrolidone, N,N-dimethylpropanamide ... N,N,N',N'-tetramethylurea, 3-methyl-2-oxazolidinone, and the like.

[0083] The content of the alkali-soluble resin (b) is preferably 10% by mass or more, more preferably 30% by mass or more, based on 100% by mass of the solid content of the positive photosensitive pigment composition in order to improve storage stability, and is preferably 90% by mass or less, more preferably 60% by mass or less in order to improve exposure sensitivity.

[0084] <Compound (c) Having a Phenolic Hydroxyl Group and a Molecular Weight of 1,000 or Less> The positive photosensitive pigment composition of the present invention further contains a compound (c) having a phenolic hydroxyl group and a molecular weight of 1,000 or less (hereinafter, may be referred to as compound (c)). By containing compound (c), alkaline developability can be improved and good exposure sensitivity can be obtained in halftone processing. From the viewpoint of alkaline developability, the molecular weight of compound (c) is preferably 800 or less, more preferably 600 or less.

[0085] In the positive photosensitive pigment composition of the present invention, compound (c) contains compound (c1) having an alkyl group having 5 to 20 carbon atoms. By including compound (c1), it is possible to prevent insoluble pigment (a) in the film that has dissolved during the development step from reattaching to the pattern openings, and it is possible to form a pattern that is free of residues derived from pigment (a) in the openings. Even when the content of pigment (a) is high, it is possible to prevent residues in the pattern openings, so this is particularly effective when halftone processing a pixel division layer that has high light-blocking properties.

[0086] Specific examples of compound (c1) include 2-hydroxy-4-pentyloxybenzophenone, 2-hydroxy-4-hexyloxybenzophenone, 2-hydroxy-4-heptyloxybenzophenone, 2-hydroxy-4-octyloxybenzophenone, 2-hydroxy-4-nonyloxybenzophenone, 2-hydroxy-4-decyloxybenzophenone, 2-hydroxy-4-undecyloxybenzophenone, 2-hydroxy-4-dodecyloxybenzophenone, 2-hydroxy-4-tridecyloxybenzophenone, ...pentyloxybenzophenone, 2-hydroxy-4-pentyloxybenzophenone, 2-hydroxy-4-pentyloxybenzophenone, 2-hydroxy-4-pentyloxybenzophenone, 2-hydroxy-4-pentyloxybenzophenone, 2-hydroxy-4-pentyloxybenzophenone, 2-hydroxy-4-pentyloxybenzophenone, 2-hydroxy-4-pentyloxybenzophenone, 2-hydroxy-4-pentyloxybenzophenone, 2-hydroxy-4-pentyloxybenzophenone, 2-hydroxy-4-pentyloxybenzophenone, 2-hydroxy-4-pentyloxybenzophenone, 2-hydroxy-4-pentyloxybenzophenone, 2-hydroxy-4-pentyloxybenzophenone, 2-hydroxy-4-pentyloxybenzophenone, 2-hydroxy-4-pentyloxybenzophenone, 2-hydroxy-4-tetradecyloxybenzophenone, 2-hydroxy-4-pentadecyloxybenzophenone, 2-hydroxy-4-hexadecyloxybenzophenone, 2-hydroxy-4-heptadecyloxybenzophenone, 2-hydroxy-4-octadecyloxybenzophenone, 2-hydroxy-4-nonadecyloxybenzophenone, 2-hydroxy-4-icosyloxybenzophenone, 2-dodecyl-p-cresol, hexadecyl 3,5-di-tert-butyl-4-hydroxybenzoate, 4-pentylphenol, 4-hexyl Phenol, 4-heptylphenol, 4-octylphenol, 4-nonylphenol, 4-decylphenol, 4-undecylphenol, 4-dodecylphenol, 4-tridecylphenol, 4-tetradecylphenol, 4-pentadecylphenol, 4-hexadecylphenol, 4-heptadecylphenol, 4-octadecylphenol, 4-nonadecylphenol, 4-icosylphenol, 3-pentylphenol, 3-hexylphenol, 3-heptylphenol, 3-octylphenol, 3-nonylphenol, 3-decylphenol phenol, 3-undecylphenol, 3-dodecylphenol, 3-tridecylphenol, 3-tetradecylphenol, 3-pentadecylphenol, 3-hexadecylphenol, 3-heptadecylphenol, 3-octadecylphenol, 3-nonadecylphenol, 3-icosylphenol, 2-pentylphenol, 2-hexylphenol, 2-heptylphenol, 2-octylphenol, 2-nonylphenol, 2-decylphenol, 2-undecylphenol, 2-dodecylphenol, 2-tridecylphenol,2-tetradecylphenol, 2-pentadecylphenol, 2-hexadecylphenol, 2-heptadecylphenol, 2-octadecylphenol, 2-nonadecylphenol, 2-icosylphenol, pentyl 4-hydroxybenzoate, hexyl 4-hydroxybenzoate, heptyl 4-hydroxybenzoate, octyl 4-hydroxybenzoate, nonyl 4-hydroxybenzoate, decyl 4-hydroxybenzoate, undecyl 4-hydroxybenzoate, dodecyl 4-hydroxybenzoate, tridecyl 4-hydroxybenzoate, 4-hydroxybenzo Tetradecyl 4-hydroxybenzoate, pentadecyl 4-hydroxybenzoate, hexadecyl 4-hydroxybenzoate, heptadecyl 4-hydroxybenzoate, octadecyl 4-hydroxybenzoate, nonadecyl 4-hydroxybenzoate, eicosyl 4-hydroxybenzoate, pentyl 3-hydroxybenzoate, hexyl 3-hydroxybenzoate, heptyl 3-hydroxybenzoate, octyl 3-hydroxybenzoate, nonyl 3-hydroxybenzoate, decyl 3-hydroxybenzoate, undecyl 3-hydroxybenzoate, dodecyl 3-hydroxybenzoate, 3-hydroxy Tridecyl benzoate, tetradecyl 3-hydroxybenzoate, pentadecyl 3-hydroxybenzoate, hexadecyl 3-hydroxybenzoate, heptadecyl 3-hydroxybenzoate, octadecyl 3-hydroxybenzoate, nonadecyl 3-hydroxybenzoate, icosyl 3-hydroxybenzoate, pentyl salicylate, hexyl salicylate, heptyl salicylate, octyl salicylate, nonyl salicylate, decyl salicylate, undecyl salicylate, dodecyl salicylate, tridecyl salicylate, tetradecyl salicylate, pentadecyl salicylate, salicylic acid Hexadecyl licylate, heptadecyl salicylate, octadecyl salicylate, nonadecyl salicylate, eicosyl salicylate, pentyl 3,4-dihydroxybenzoate, hexyl 3,4-dihydroxybenzoate, heptyl 3,4-dihydroxybenzoate, octyl 3,4-dihydroxybenzoate, nonyl 3,4-dihydroxybenzoate, decyl 3,4-dihydroxybenzoate, undecyl 3,4-dihydroxybenzoate, dodecyl 3,4-dihydroxybenzoate, tridecyl 3,4-dihydroxybenzoate, tetradecyl 3,4-dihydroxybenzoate,Pentadecyl 3,4-dihydroxybenzoate, hexadecyl 3,4-dihydroxybenzoate, heptadecyl 3,4-dihydroxybenzoate, octadecyl 3,4-dihydroxybenzoate, nonadecyl 3,4-dihydroxybenzoate, icosyl 3,4-dihydroxybenzoate, pentyl 2,3-dihydroxybenzoate, hexyl 2,3-dihydroxybenzoate, heptyl 2,3-dihydroxybenzoate, octyl 2,3-dihydroxybenzoate, nonyl 2,3-dihydroxybenzoate, decyl 2,3-dihydroxybenzoate, 2,3-dihydroxybenzoic acid Undecyl 2,3-dihydroxybenzoate, Dodecyl 2,3-dihydroxybenzoate, Tridecyl 2,3-dihydroxybenzoate, Tetradecyl 2,3-dihydroxybenzoate, Pentadecyl 2,3-dihydroxybenzoate, Hexadecyl 2,3-dihydroxybenzoate, Heptadecyl 2,3-dihydroxybenzoate, Octadecyl 2,3-dihydroxybenzoate, Nonadecyl 2,3-dihydroxybenzoate, Eicosyl 2,3-dihydroxybenzoate, Pentyl 2,4-dihydroxybenzoate, Hexyl 2,4-dihydroxybenzoate, Heptyl 2,4-dihydroxybenzoate 2,4-dihydroxybenzoic acid octyl, 2,4-dihydroxybenzoic acid nonyl, 2,4-dihydroxybenzoic acid decyl, 2,4-dihydroxybenzoic acid undecyl, 2,4-dihydroxybenzoic acid dodecyl, 2,4-dihydroxybenzoic acid tridecyl, 2,4-dihydroxybenzoic acid tetradecyl, 2,4-dihydroxybenzoic acid pentadecyl, 2,4-dihydroxybenzoic acid hexadecyl, 2,4-dihydroxybenzoic acid heptadecyl, 2,4-dihydroxybenzoic acid octadecyl, 2,4-dihydroxybenzoic acid nonadecyl, 2,4-dihydroxybenzoic acid eicosyl hydroxybenzoate, pentyl 2,5-dihydroxybenzoate, hexyl 2,5-dihydroxybenzoate, heptyl 2,5-dihydroxybenzoate, octyl 2,5-dihydroxybenzoate, nonyl 2,5-dihydroxybenzoate, decyl 2,5-dihydroxybenzoate, undecyl 2,5-dihydroxybenzoate, dodecyl 2,5-dihydroxybenzoate, tridecyl 2,5-dihydroxybenzoate, tetradecyl 2,5-dihydroxybenzoate, pentadecyl 2,5-dihydroxybenzoate, hexadecyl 2,5-dihydroxybenzoate,Examples of the gallate include heptadecyl 2,5-dihydroxybenzoate, octadecyl 2,5-dihydroxybenzoate, nonadecyl 2,5-dihydroxybenzoate, icosyl 2,5-dihydroxybenzoate, pentyl gallate, hexyl gallate, heptyl gallate, octyl gallate, nonyl gallate, decyl gallate, undecyl gallate, dodecyl gallate, tridecyl gallate, tetradecyl gallate, pentadecyl gallate, hexadecyl gallate, heptadecyl gallate, octadecyl gallate, nonadecyl gallate, and icosyl gallate.

[0087] The compound (c1) preferably contains a compound represented by formula (1) in order to suppress development residues.

[0088]

[0089] In formula (1), R 1 represents —NH— or an oxygen atom. 2 represents an alkyl group having 5 to 20 carbon atoms. 3 , R 4 , R 5 , R 6 and R 7 each independently represents a hydrogen atom, an alkyl group, or a hydroxyl group. 3 , R 4 , R 5 , R 6 and R 7 The total number of hydroxyl groups therein is 1 to 3.

[0090] Furthermore, it is more preferable that the compound (c1) has an alkyl group having 12 to 18 carbon atoms in terms of suppressing pigment residue.

[0091] The compound (c) preferably contains a compound (c2) that does not contain an alkyl group having 5 to 20 carbon atoms and that contains an aryl group substituted with three or more phenolic hydroxyl groups. By containing the compound (c2), insoluble residues at the edge of the pattern opening can be suppressed during halftone processing.

[0092] Examples of compound (c2) include phloroglucinol, pyrogallol, 1,2,4-trihydroxybenzene, 2,4,5-trihydroxybenzaldehyde, 2,3,4-trihydroxybenzaldehyde, 3,4,5-trihydroxybenzaldehyde, gallacetophenone, 2,3,4-trihydroxybenzoic acid, gallic acid, methyl gallate, ethyl gallate, propyl gallate, 2,3,4-trihydroxybenzophenone, 2,3,4,4'-tetrahydroxybenzophenone, 4,4'-isopropylidenedipyrogallol, 1,2,3,4-tetrahydroxybenzene, 1,2,3,5-tetrahydroxybenzene, 1,2,4,5-tetrahydroxybenzene, and leucoquinizarin.

[0093] It is more preferable that compound (c2) is a compound represented by formula (40), since this can suppress insoluble residues at the edge of the pattern opening during halftone processing, as well as minute residues of less than 0.1 μm in size within the opening.

[0094]

[0095] In formula (40), n 24 is 3 to 6. Examples of the compound represented by formula (40) include phloroglucinol, pyrogallol, 1,2,4-trihydroxybenzene, 1,2,3,5-tetrahydroxybenzene, and hexahydroxybenzene.

[0096] As the compound (c) in the positive photosensitive pigment composition of the present invention, any known compound other than the compound (c1) and the compound (c2) can be used. For example, a compound that can be converted by heating into a compound having an absorption maximum in a wavelength region of 350 to 500 nm in a wavelength region of 350 to 780 nm can be used. Examples of such compounds include 4,4',4",4""-(1,4-phenylenedimethylidene)tetrakisphenol (maximum absorption wavelength after heat treatment: 440 nm), 4,4',4"-trihydroxytriphenylmethane represented by formula (53) (maximum absorption wavelength after heat treatment: 460 nm), and 4-[bis(4-hydroxyphenyl)methyl]2-methoxyphenol (maximum absorption wavelength after heat treatment: 470 nm). As described above, pigment (a) has a higher transmittance in the wavelength region of 410 to 440 nm than in the wavelength region of 500 to 650 nm. Therefore, by containing compound (c) that is converted into a compound having a maximum absorption wavelength in the wavelength region of 350 to 500 nm, the maximum transmittance in the wavelength region of 410 to 440 nm of the pixel dividing layer obtained after heat treatment can be preferably lowered.

[0097] The content of compound (c) is preferably 1% by mass or more, more preferably 5% by mass or more, relative to 100% by mass of the solid content of the positive photosensitive pigment composition, from the viewpoint of improving the exposure sensitivity of halftone processability, and is preferably 20% by mass or less, more preferably 15% by mass or less, from the viewpoint of suppressing excessive alkali developability.

[0098] The content of compound (c1) in compound (c) is preferably 15 to 70 mass% in compound (c), and the content of compound (c2) is preferably 30 to 85 mass% in compound (c). The content of compound (c1) is preferably 70 mass% or less in terms of exposure sensitivity, and preferably 15 mass% or more in terms of suppressing pigment residue. The content of compound (c2) is preferably 85 mass% or less in terms of exposure sensitivity, and preferably 30 mass% or more in terms of suppressing insoluble matter residue at the edge of the pattern opening. Therefore, when the contents of compound (c1) and compound (c2) are within the above ranges, halftone processing can be performed with high exposure sensitivity, and both pigment residue and insoluble matter residue at the edge of the pattern opening can be suppressed.

[0099] When compound (c2) is a compound represented by formula (40), the ratio mc1 / mc2 of the content (mass) of compound (c1) mc1 to the content (mass) of compound (c2) mc2 is preferably 0.3 or more and less than 1.0. By keeping the ratio mc1 / mc2 within this range, minute residues less than 0.1 μm in the opening can be particularly suppressed.

[0100] <Photoacid Generator (d)> The positive photosensitive pigment composition of the present invention further contains a photoacid generator (d). By including the photoacid generator (d), acid is generated in the light-irradiated areas, increasing the solubility of the light-irradiated areas in an alkaline aqueous solution, thereby obtaining a positive pattern in which the light-irradiated areas dissolve. In addition, the amount of acid generated in the film can be controlled by adjusting the exposure dose, which has the effect of making the solubility in an alkaline developer of the exposed areas of the film exposed to a low exposure dose through a halftone exposure mask relatively lower than the solubility in an alkaline developer of the exposed areas of the film exposed to a high exposure dose, making it possible to form a pattern having steps by positive halftone processing.

[0101] The photoacid generator (d) may be, for example, a quinone diazide compound. The positive photosensitive pigment composition of the present invention preferably contains two or more types of photoacid generator (d). When two or more types are contained, a positive photosensitive pigment composition with higher sensitivity can be obtained.

[0102] The quinone diazide compound may include a compound in which a sulfonic acid of quinone diazide is bonded to a polyhydroxy compound via an ester bond, a compound in which a sulfonic acid of quinone diazide is bonded to a polyamino compound via a sulfonamide bond, or a compound in which a sulfonic acid of quinone diazide is bonded to a polyhydroxypolyamino compound via an ester bond and / or a sulfonamide bond.

[0103] As the quinone diazide structure, either a 5-naphthoquinone diazide sulfonyl group or a 4-naphthoquinone diazide sulfonyl group is preferably used. A naphthoquinone diazide sulfonyl ester compound having both a 4-naphthoquinone diazide sulfonyl group and a 5-naphthoquinone diazide sulfonyl group in the same molecule may be contained, or a 4-naphthoquinone diazide sulfonyl ester compound and a 5-naphthoquinone diazide sulfonyl ester compound may be contained. The 4-naphthoquinone diazide sulfonyl ester compound has absorption in the i-line region of a mercury lamp and is suitable for i-line exposure. The 5-naphthoquinone diazide sulfonyl ester compound has absorption extending into the g-line region of a mercury lamp and is suitable for g-line exposure. It is preferable to select a 4-naphthoquinone diazide sulfonyl ester compound or a 5-naphthoquinone diazide sulfonyl ester compound depending on the wavelength of exposure.

[0104] The quinone diazide compound can be synthesized by any esterification reaction of a compound having a phenolic hydroxyl group and a quinone diazide sulfonic acid compound. The use of such a quinone diazide compound further improves resolution, sensitivity, and film retention.

[0105] The content of the photoacid generator (d) is preferably 1% by mass or more, more preferably 5% by mass or more, based on 100% by mass of the solid content of the positive photosensitive pigment composition, in order to generate a necessary and sufficient amount of acid in the film and thereby improve the exposure sensitivity, and is preferably 30% by mass or less, more preferably 20% by mass or less, in order to suppress excessive absorption of the exposure light on the film surface and thereby improve the exposure sensitivity.

[0106] <Solvent (e)> The positive photosensitive pigment composition of the present invention further contains a solvent (e), which not only contributes to improving storage stability as a dispersion medium for the pigment (a), but also improves the coatability of the positive photosensitive pigment composition, thereby enhancing the smoothness of the prebaked film described below and improving halftone processability.

[0107] Examples of the solvent (e) include ether-based solvents, glycol-based solvents, acetate-based solvents, ketone-based solvents, lactone-based solvents, aromatic carbon-based solvents, and amide-based solvents.

[0108] Examples of ether-based solvents include ethylene glycol monomethyl ether, ethylene glycol mono-n-propyl ether, ethylene glycol mono-n-butyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol mono-n-propyl ether, diethylene glycol mono-n-butyl ether, propylene glycol monomethyl ether (hereinafter referred to as "PGME"), propylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, propylene glycol mono-n-butyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol mono-n-propyl ether, dipropylene glycol mono-n-butyl ether, tripropylene glycol monomethyl ether, and tripropylene glycol monoethyl ether. Examples of glycol-based solvents include ethylene glycol, propylene glycol, diethylene glycol, and dipropylene glycol. Examples of acetate-based solvents include ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate (hereinafter referred to as "PGMEA"), propylene glycol monoethyl ether acetate, methyl lactate, ethyl lactate, and 3-methoxybutyl acetate (hereinafter referred to as "MBA"). Examples of ketone-based solvents include methyl ethyl ketone, diisobutyl ketone, cyclohexanone, 2-heptanone, and 3-heptanone. Examples of lactone-based solvents include γ-butyrolactone and γ-valerolactone. Examples of aromatic carbon-based solvents include toluene, xylene, and benzene. Examples of amide-based solvents include N-methylpyrrolidone (hereinafter referred to as "NMP"), N,N-dimethylformamide, and N,N-dimethylacetamide. Among these, in order to improve storage stability, it is preferable to contain an ether-based solvent and / or an acetate-based solvent, and it is more preferable to further contain a lactone-based solvent.

[0109] The content of the solvent (e) is preferably 30% by mass or more, more preferably 50% by mass or more, relative to 100% by mass of the positive photosensitive pigment composition in order to improve storage stability, and is preferably 99% by mass or less, more preferably 95% by mass or less in order to improve the smoothness of the prebaked film.

[0110] In order to improve storage stability, the contents of the aromatic hydrocarbon solvent and the amide solvent are preferably 0.5% by mass or less, respectively, relative to 100% by mass of the positive photosensitive pigment composition. Furthermore, the storage stability may be further improved by including 0.01 to 0.5% by mass of water relative to 100% by mass of the positive photosensitive pigment composition.

[0111] <Organic dye particles (f) having a sulfo group> The positive photosensitive pigment composition of the present invention preferably further contains organic dye particles (f) having a sulfo group in order to improve halftone processability and storage stability. The sulfo group here refers to an organic dye particle having a group selected from the group consisting of —SO 3 In addition to H, the proton may be dissociated in the positive photosensitive pigment composition, and —SO 3 - Includes.

[0112] The organic dye referred to here refers to organic dyes and organic pigments that have absorption at least in the visible light region. The organic dye particles (f) are present in the positive photosensitive pigment composition as insoluble fine particles dispersed therein. The form of the organic dye particles (f) can be controlled by adjusting the solvent (e) relative to the total number of sulfo groups contained in the molecules of the organic dyes belonging to the organic dye particles (f). Furthermore, the organic dye particles (f) may be contained as a surface treatment agent for the pigment (a), or the pigment (a) and the organic dye particles (f) may form a mixed crystal. In the case of a surface treatment agent or a mixed crystal, it is defined as a mixture of the pigment (a) and the organic dye particles (f). An organic dye having a triphenodioxazine skeleton and a sulfo group is defined as organic dye particles (f).

[0113] The method for producing the organic dye particles (f) is not particularly limited, and the organic dye particles (f) may be a pigment derivative obtained by derivatizing a so-called organic pigment, or may be an organic dye synthesized using an intermediate compound having a sulfo group as a raw material, without going through the form of an organic pigment.

[0114] Examples of the organic dye particles (f) include triphenodioxazine dyes, perylene bisimide dyes, anthraquinone dyes, perinone dyes, phthalocyanine dyes, quinacridone dyes, benzofuranone dyes, and flavanthrone dyes. Among these, triphenodioxazine dyes, perylene bisimide dyes, and anthraquinone dyes are more preferred in terms of improving halftone processability and storage stability.

[0115] That is, in the positive photosensitive pigment composition of the present invention, the organic dye particles (f) more preferably contain at least one dye selected from the group consisting of triphenodioxazine dyes, perylene bisimide dyes, and anthraquinone dyes.

[0116] The sulfo group contained in the organic dye particles (f) is preferably a sulfo group bonded to a carbon atom constituting an aromatic ring, in order to achieve both halftone processability and storage stability. Examples of organic groups containing a sulfo group bonded to a carbon atom constituting an aromatic ring include a sulfophenyl group, a disulfophenyl group, a carboxy-sulfophenyl group, a methyl-sulfophenyl group, a methoxy-sulfophenyl group, a sulfonaphthyl group, a disulfonaphthyl group, a carboxy-sulfonaphthyl group, a methyl-sulfonaphthyl group, and a methoxy-sulfonaphthyl group.

[0117] Examples of triphenodioxazine dyes belonging to the organic dye particles (f) include compounds represented by formula (19) and compounds represented by formula (20).

[0118]

[0119] In formula (19), R 35 and R 36 R each independently represents —NH— or an oxygen atom. 37 and R 38R each independently represents an alkyl group having 1 to 4 carbon atoms. 39 and R 40 R each independently represents -NH- or -CONH-. 41 , R 42 , R 45 and R 46 are each independently -SO 3 H, -SO 3 - , —COOH or —COO - Represents R 43 and R 44 each independently represents an alkyl group having 1 to 4 carbon atoms or an alkoxy group having 1 to 4 carbon atoms. 1 and n 2 are integers, each independently representing 0 or 1. 3 , n 4 , n 5 and n 6 are integers, each independently representing 0 to 2. 7 is an integer and represents 0 or 1. 1 , n 3 and n 7 The sum of n is 2 or less, 2 , n 4 and n 7 The sum of n is 2 or less. 7 If is 0, then n 3 and n 4 The sum of n is 1 to 3. 7 If is 1, then n 3 , n 4 , n 5 and n 6 The sum is 1 to 3.

[0120]

[0121] In formula (20), R 47 and R 48 R each independently represents —NH— or an oxygen atom. 49 and R 50 R each independently represents an alkyl group having 1 to 4 carbon atoms. 51 , R 52 , R 53 and R 54are each independently -SO 3 H, -SO 3 - , —COOH or —COO - Represents R 55 and R 56 Each of n independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 8 , n 9 , n 10 and n 11 are integers, each independently representing 0 or 1. 8 , n 9 , n 10 and n 11 The sum is 1 to 3.

[0122] Examples of the perylene bisimide dyes belonging to the organic dye particles (f) include compounds represented by formula (21) and compounds represented by formula (22).

[0123]

[0124] In formula (21), R 57 and R 58 R each independently represents a phenylene group substituted with an alkyl group having 1 to 6 carbon atoms, a phenylene group substituted with an alkoxy group having 1 to 6 carbon atoms, an unsubstituted phenylene group, a naphthylene group substituted with an alkyl group having 1 to 6 carbon atoms, a naphthylene group substituted with an alkoxy group having 1 to 6 carbon atoms, or an unsubstituted naphthylene group. 59 and R 60 are each independently -SO 3 H, -SO 3 - , —COOH or —COO - represents n 12 and n 13 is an integer from 0 to 2. 12 and n 13 The sum is 1 to 3.

[0125]

[0126] In formula (22), R 61 and R 62 R each independently represents an alkyl group having 1 to 6 carbon atoms. 63 and R64 are each independently -SO 3 H, -SO 3 - , —COOH or —COO - represents n 14 and n 15 is an integer from 0 to 2. 14 and n 15 The sum is 1 to 3.

[0127] Examples of the anthraquinone dyes belonging to the organic dye particles (f) include compounds represented by formula (23) and compounds represented by formula (24).

[0128]

[0129] In formula (23), R 65 and R 66 represents an alkyl group having 1 to 3 carbon atoms. 16 and n 17 is an integer from 0 to 3. 67 and R 68 are each independently -SO 3 H or -SO 3 - represents n 18 and n 19 is an integer from 0 to 2. 18 and n 19 The sum is 1 to 3.

[0130]

[0131] In formula (24), R 69 and R 70 represents an alkyl group having 1 to 3 carbon atoms. 20 and n 21 is an integer from 0 to 3. 71 and R 72 are each independently —COOH or —COO - Represents R 73 and R 74 represents an alkyl group having 1 to 3 carbon atoms. 22 and n 23 is an integer and represents 0 or 1.

[0132] When the positive photosensitive pigment composition of the present invention contains organic colorant particles (f), the content of the organic colorant particles (f) is preferably 5 to 50 parts by mass per 100 parts by mass of the pigment (a), in order to achieve both halftone processability and storage stability.

[0133] The positive photosensitive pigment composition of the present invention may further contain a thermal crosslinking agent (g). The inclusion of the thermal crosslinking agent (g) facilitates adjustment of the optimum development time in the development step described below within an appropriate range, and may also improve the film strength of the pixel dividing layer and spacer layer. The thermal crosslinking agent (g) is preferably a compound having two or more alkoxymethyl groups or epoxy groups in the molecule. Examples of the alkoxymethyl group include a methoxymethyl group, an ethoxymethyl group, a propoxymethyl group, and a butoxymethyl group.

[0134] Examples of compounds having two or more alkoxymethyl groups in the molecule include HMOM-TPHAP, DML-PC, DML-PEP, DML-OC, and DML-POP (all manufactured by Honshu Chemical Industry Co., Ltd.), and NIKALAC (registered trademark) MX-390, MX-290, MX-280, MX-270, MW-100LM, and MX-750LM (all manufactured by Sanwa Chemical Co., Ltd.).

[0135] Examples of compounds having two or more epoxy groups in the molecule include TEPIC-S, TEPIC-PAS, TEPIC-VL, and TEPIC-UC (all manufactured by Nissan Chemical Industries, Ltd.), XD-1000, XD-1000-H, XD-1000-2L, and NC-3000 (all manufactured by Nippon Kayaku Co., Ltd.), TECHMORE VG3101L (manufactured by Printec Co., Ltd.), TR-FR-201 (manufactured by Tronly), KR-470, X-40-2678, and X-40-2669 (all manufactured by Shin-Etsu Chemical Co., Ltd.).

[0136] The positive photosensitive pigment composition of the present invention may contain, if necessary, a nonionic surfactant as a leveling agent, or a silane coupling agent or surfactant as an adhesion improver to the substrate surface.

[0137] The chemical structures of the compounds belonging to the aforementioned pigment (a), alkali-soluble resin (b), compound (c), photoacid generator (d), solvent (e), organic dye particles (f), and thermal crosslinker (g) can be analyzed by combining known analytical techniques such as time-of-flight secondary ion mass spectrometry (TOF-SIMS), time-of-flight mass spectrometry (TOF-MS), nuclear magnetic resonance (NMR), liquid chromatography mass spectrometry (LC-MS), gas chromatography mass spectrometry (GC-MS), ICP mass spectrometry, infrared absorption spectrometry, and X-ray diffraction using the positive photosensitive pigment composition of the present invention as a sample. In particular, for the pigment (a) and the organic dye particles (f), the positive photosensitive pigment composition may be centrifuged, and the concentrate obtained as the filtrate may be analyzed as a sample to improve identification accuracy. On the other hand, for the alkali-soluble resin (b), compound (c), photoacid generator (d), and thermal crosslinker (g), the filtrate obtained by filtering the supernatant after centrifugation may be analyzed as a sample to improve identification accuracy.

[0138] The method for preparing the positive photosensitive pigment composition is not particularly limited, but examples include a method in which a pigment dispersion containing the pigment (a), the alkali-soluble resin (b), the solvent (e), and, if necessary, the organic colorant particles (f) is prepared in advance by wet dispersion treatment, and then the compound (c), the photoacid generator (d), and, if necessary, the thermal crosslinker (g) and other components are mixed and stirred with the pigment dispersion, and if necessary, filtered. In particular, it is desirable to use the alkali-soluble resin (b) in the production of the pigment dispersion, because the interaction with the pigment (a) makes it easier to achieve even greater improvement in storage stability.

[0139] The disperser used for wet dispersion treatment may be a wet media disperser or a wet medialess disperser, but the use of a wet media disperser is desirable due to its excellent dispersion treatment speed and economical advantages. Examples of wet media dispersers include bead mills such as "Levomill" (registered trademark) (manufactured by Asada Iron Works Co., Ltd.), "Nano Getter" (registered trademark) (manufactured by Ashizawa Finetech Co., Ltd.), "DYNO-MILL" (registered trademark) (manufactured by Willy A. Bachofen), "Spike Mill" (registered trademark) (manufactured by Inoue Manufacturing Co., Ltd.), "Sand Grinder" (registered trademark) (manufactured by DuPont), "Ultra Apex Mill" (registered trademark) (manufactured by Hiroshima Metal & Machinery Co., Ltd.), and "NEO-Alpha Mill" (registered trademark) (manufactured by AIMEX Co., Ltd.). The media material is preferably ceramic beads such as zirconia, and their diameter is preferably 0.03 to 0.5 mmφ. An example of a commercially available product is "Treceram" (registered trademark) (manufactured by Toray Industries, Inc.).

[0140] The D90 (50% cumulative secondary particle diameter) in the particle size distribution of the particle components in the positive photosensitive pigment composition, measured by dynamic light scattering based on light scattering intensity, is preferably 150 nm or more in order to improve storage stability. On the other hand, in order to improve halftone processability, it is preferably 300 nm or less. D90 refers to the value measured on a particle size distribution measurement sample. The particle size distribution measurement sample refers to a measurement object obtained by mixing equal amounts of dilution solvent into a positive photosensitive pigment composition in three batches so that the ratio of positive photosensitive pigment composition to dilution solvent is 1:99 (mass ratio), and stirring the mixture on a shaker for 10 minutes. The dilution solvent used is an organic solvent with the same composition as solvent (e) contained in the positive photosensitive pigment composition. The particle size distribution referred to here can be measured using a particle size distribution measuring device SZ-100 (manufactured by Horiba, Ltd.) using a dynamic light scattering method, and D90 means a particle size (nm) corresponding to 90% cumulatively accumulated toward the larger particle size side on a cumulative particle size distribution curve, with the smaller particle size side being the base point (0%).

[0141] The cured product of the present invention is a product obtained by curing the positive-type photosensitive pigment composition of the present invention. That is, the cured product of the present invention is derived from the positive-type photosensitive pigment composition of the present invention. The cured product here refers to a product obtained by heating the positive-type photosensitive pigment composition at a temperature of 200°C to 400°C under atmospheric pressure for 10 minutes or longer. By heat-treating the positive-type photosensitive pigment composition of the present invention, components with low heat resistance can be removed, thereby further improving the heat resistance and chemical resistance. In particular, when the positive-type photosensitive pigment composition of the present invention contains a polyimide precursor, a polybenzoxazole precursor, a copolymer thereof, or a copolymer thereof with a polyimide, the heat treatment forms imide rings and oxazole rings, thereby further improving the heat resistance and chemical resistance.

[0142] The positive photosensitive pigment composition and cured product of the present invention are suitable for use as surface protection layers and interlayer insulating layers for semiconductor elements, insulating layers for organic electroluminescence (EL) elements, planarizing layers for thin film transistor (TFT) substrates used to drive display devices using organic EL elements, wiring protection insulating layers for circuit boards, on-chip microlenses for solid-state imaging devices, and planarizing layers for various display devices and solid-state imaging devices. In other words, the organic EL display device of the present invention comprises the cured product of the present invention. For example, the composition is suitable as a surface protection layer or interlayer insulating layer for MRAM with low heat resistance, polymer memory (Polymer Ferroelectric RAM: PFRAM) and phase change memory (Phase Change RAM: PCRAM, Ovonics Unified Memory: OUM), which are promising next-generation memories, and the like. The present invention can also be used as an insulating layer in a display device including a first electrode formed on a substrate and a second electrode provided opposite the first electrode, such as an LCD, an ECD, an ELD, or a display device using an organic electroluminescent element (organic electroluminescent device).

[0143] The organic EL display device of the present invention comprises a cured product. For example, an organic EL display device having a drive circuit, a TFT planarizing layer, a first electrode, a pixel dividing layer, a light-emitting layer, and a second electrode on a substrate is preferably provided with a cured product of the positive photosensitive pigment composition of the present invention. The form of the cured product in the organic EL display device is not particularly limited, but examples include a pixel dividing layer and a TFT planarizing layer. When provided with a pixel dividing layer and / or a TFT planarizing layer containing a cured product of the positive photosensitive pigment composition, the organic EL display device of the present invention has an excellent function of suppressing external light reflection, and exhibits the technical effect of excellent visibility without the need for a polarizing plate. Components other than the cured product of the positive photosensitive pigment composition provided in the organic EL display device of the present invention include, for example, moisture mixed in during the process of forming the cured product, and Na mixed into the cured product originating from the underlying substrate or electrodes. + , Ag + Examples of metal ions include:

[0144] A preferred embodiment in which the cured product of the present invention is used as a pixel dividing layer in an organic EL display device will be described below.

[0145] The optical density per 1.0 μm of film thickness of the pixel division layer is preferably 0.8 or more, more preferably 1.0 or more, in order to suppress external light reflection and enhance the value of the display device. From the viewpoint of halftone processing, it is preferably 1.5 or less, more preferably 1.3 or less.

[0146] The optical density refers to the value obtained by measuring the incident light intensity and transmitted light intensity of a pixel division layer formed on a transparent substrate to a thickness of 1.5 μm using an optical densitometer X-Rite 361T (manufactured by X-Rite Corporation), calculating the value using the following formula, and dividing the calculated value by 1.5, which is the film thickness value. The higher the optical density, the higher the light-blocking property. As the transparent substrate, a transparent glass substrate "Tempax (manufactured by AGC Technoglass Co., Ltd.)" can be preferably used. Optical density = log 10 (I 0 / I) In the above formula, I 0 : incident light intensity, I: transmitted light intensity.

[0147] In order to reduce the contact area with the deposition mask during pattern deposition of the light-emitting layer, thereby improving yield and simultaneously achieving exposure sensitivity, the thickness of the thick portion of the stepped pixel division layer is preferably 2.5 to 4.0 μm, and the thickness of the thin portion is preferably 1.0 to 2.5 μm. The thicknesses of the thick portion and the thin portion referred to here refer to the thickness of the flat portion, excluding the thickness of the inclined portion located at the end of the film. The difference in thickness between the thick portion and the thin portion is preferably 1.0 to 2.0 μm. An opening may be formed only in the thin portion, and the thick portion may be locally arranged in a spacer-like manner. The cross-sectional taper angle of the inclined portion located at the end of the thin portion of the stepped pixel division layer is preferably 50° or less, more preferably 40° or less, in order to prevent electrode disconnection and avoid the occurrence of non-illuminated pixels. The thickness is preferably 15° or more, more preferably 20° or more, in order to prevent a decrease in light-blocking property at the end of the thin portion.

[0148] A preferred method for forming a pixel division layer having steps includes a coating step of applying a positive photosensitive pigment composition to obtain a coating film, a pre-baking step of heating the coating film to obtain a pre-baked film, an exposure step of pattern-exposing the film to actinic rays through a positive half-tone exposure mask to obtain an exposed film having exposed areas, semi-exposed areas, and unexposed areas within its surface, a development step of developing the film using an alkaline developer to remove part of the semi-exposed and unexposed areas in addition to the exposed areas to obtain a developed film, and a curing step of thermally curing the film by heating to obtain a cured product.

[0149] As a coating device used in the coating step, a spin coater or a slit coater can be preferably used because of its excellent thin film coating ability. After coating, pin gap pre-baking or contact pre-baking may be performed.

[0150] The pre-baking temperature in the pre-baking step is preferably 50 to 150°C, and the pre-baking time is preferably 30 seconds to 5 minutes. When pixel division layers having steps are formed in one step, the thickness of the pre-baked film is preferably 3.5 to 5.5 μm. When near-infrared alignment is performed in the exposure step described below, the maximum transmittance of the pre-baked film of the positive photosensitive pigment composition at a wavelength of 800 to 1,300 nm is preferably 20% or more, and more preferably 30% or more, in order to improve positional accuracy.

[0151] Examples of exposure devices used in the exposure step include a stepper, a mirror projection mask aligner (MPA), and a parallel light mask aligner (PLA). Examples of active actinic rays irradiated during exposure include the j-line (wavelength 313 nm), i-line (wavelength 365 nm), h-line (wavelength 405 nm), or g-line (wavelength 436 nm) from an ultra-high pressure mercury lamp. Mixed rays containing at least the h-line are preferred, and mixed rays containing the g-line, h-line, and i-line are more preferred. A positive halftone exposure mask preferably has a fully transparent portion, a semi-transparent portion, and a shielding portion within the substrate plane, and is designed so that when the exposure amount in the fully transparent portion is 100% and the exposure amount in the shielding portion is 0%, the exposure amount in the semi-transparent portion is 10 to 50%.

[0152] The exposed portions of the exposed film refer to the portions that have been pattern-exposed through the fully transparent portions of the exposure mask, the partially exposed portions refer to the portions that have been pattern-exposed through the semi-transparent portions of the exposure mask, and the unexposed portions refer to the portions that have not been exposed due to the shielding portions of the exposure mask. In the pixel division layer having steps obtained after the curing step, these portions become the openings, thin film portions, and thick film portions, respectively.

[0153] Examples of development methods used in the development step include showering, dipping, and puddling, and include a method in which the exposed film is immersed for 10 seconds to 3 minutes. The puddling method is preferred for improving halftone processability. A 0.4 to 2.5 wt% aqueous solution of tetramethylammonium hydroxide (hereinafter referred to as "TMAH") is preferred as the alkaline developer, and a commercially available example is 2.38 wt% TMAH (manufactured by Tama Chemicals Co., Ltd.). After the development step, a cleaning treatment using a shower of deionized water and / or a water-removing treatment using air jets may be performed. To improve the in-plane thickness uniformity of the developed film, it is preferable to set the development time so that the film thickness of the thick film portion (unexposed portion) of the developed film having steps is 1.0 μm or less. To improve exposure sensitivity, it is preferable to set the development time so that the film thickness is 0.5 μm or more. Furthermore, the developed film obtained may be irradiated with exposure light again as a second exposure step to control the fluidity of the film in the curing step.

[0154] In the curing step, the developed film is thermally cured by heating, and the developer and moisture remaining in the film are evaporated to obtain a cured product. Examples of heating devices include a hot air oven and an IR oven, and the heating atmosphere can be nitrogen or air. The heating temperature is preferably 200 to 350°C under atmospheric pressure, more preferably 220 to 280°C.

[0155] The organic EL display device of the present invention has the advantageous technical effect of eliminating dark spots within pixels. The term "dark spots" refers to granular, localized, non-luminescent regions that are unevenly arranged within a pixel when the organic EL display device is in operation. The major axis of dark spots originating from pigment residues increases to a size equal to or greater than the major axis of the pigment residues themselves, inhibiting light emission. Therefore, the more pronounced the dark spots, the lower the luminance and the lower the value of the display device.

[0156] FIG. 1 shows a cross-sectional view of a TFT substrate in an organic EL display device that is a specific example of an embodiment of the present invention.

[0157] Bottom-gate or top-gate thin film transistors 1 (hereinafter abbreviated as TFT1) are arranged in a matrix on the surface of a substrate 6. A TFT insulating layer 3 is formed to cover the TFT1 and the wiring 2 connected to the TFT1. Furthermore, a planarization layer 4 is formed on the surface of the TFT insulating layer 3, and contact holes 7 are formed in the planarization layer 4 to connect first electrodes 5 to the wiring 2. First electrodes 5 are patterned on the surface of the planarization layer 4 and connected to the wiring 2. A pixel division layer 8 is formed surrounding the periphery of the pattern of the first electrodes 5. The pixel division layer 8 has openings, in which light-emitting pixels 9 containing an organic EL light-emitting material are formed. A second electrode 10 is formed to cover the pixel division layer 8 and the light-emitting pixels 9. After sealing the TFT substrate having the above layered structure under vacuum, applying a voltage to the light-emitting pixel portions can cause the device to emit light as an organic EL display device. The shape of the openings in the pixel division layer 8 is not particularly limited and may be square, rectangular, or elliptical. The width of the opening may be determined appropriately depending on the size of the light-emitting pixel 9 described later, and the minor axis may be, for example, 10 to 50 μm.

[0158] In the organic EL display device of the present invention, the pixel dividing layer preferably has thick portions with a thickness of 2.5 to 4.0 μm and thin portions with a thickness of 1.0 to 2.5 μm, and has portions where the difference in thickness between the thick portions and the thin portions is 1.0 μm or more. The thick portions have a spacer effect, reducing the contact area with the deposition mask when forming the light-emitting pixels 9, thereby improving production yield and preventing defects in the organic EL elements and suppressing the occurrence of non-light-emitting pixels.

[0159] The emission peak wavelength of the light-emitting pixel 9 is not particularly limited. For example, a configuration in which different types of pixels having emission peak wavelengths in the three primary colors of light, blue, red, and green, are arranged on the entire surface can be used. The peak wavelength in the red region can be 560 to 700 nm, the peak wavelength in the blue region can be 420 to 480 nm, and the peak wavelength in the green region can be 500 to 550 nm. Separate laminated members, such as blue, red, and green color filters, and a black matrix separating them, can be combined and arranged on the front surface of the display unit. The organic EL light-emitting material constituting the light-emitting pixel 9 can be suitably a material that combines a light-emitting layer with a hole transport layer and / or an electron transport layer. A mask vapor deposition method can be used as a method for patterning the light-emitting pixel 9. The mask vapor deposition method is a method in which an organic compound is vapor-deposited and patterned using a vapor deposition mask. Specifically, a vapor deposition method can be performed by placing a vapor deposition mask with openings in the desired pattern on the substrate side. Examples of vapor deposition masks used to form high-definition light-emitting pixels include the vapor deposition mask disclosed in JP-A-2019-163543.

[0160] The first electrode 5 can be made of conductive metal oxides such as indium tin oxide (ITO) and indium zinc oxide (IZO). Among these, ITO is preferred due to its excellent transparency and conductivity. A method for patterning ITO involves forming an ITO film over the entire surface by sputtering, then patterning a positive etching resist material by photolithography to obtain a resist pattern on the ITO film, and then removing only the ITO film in the areas where the resist pattern is not formed with an etching solution. The resist pattern is then removed with a resist stripper, and if necessary, heat treatment is performed to achieve the desired crystallinity. A positive photosensitive pigment composition containing an alkali-soluble novolac resin can be used as the positive etching resist material. As the etching solution, an aqueous solution containing nitric acid and hydrochloric acid or an aqueous solution of oxalic acid can be used, and commercially available products include, for example, ITO-101N (manufactured by Kanto Chemical Co., Ltd.), "Sclean (registered trademark)" IS-2, and "Sclean (registered trademark)" IS-3 (all manufactured by Sasaki Chemical Co., Ltd.). As the resist stripping solution, an organic amine-based aqueous solution can be used, and commercially available products include, for example, "Anlast (registered trademark)" M6, M6B, TN-1-5, and M71-2 (all manufactured by Miwa Pure Chemical Research Institute). When the organic EL display device of the present invention is a top-emission organic EL display device, the first electrode 5 may have a laminated structure of ITO / silver alloy / ITO in order to improve light reflectivity and adhesion to the substrate.

[0161] The second electrode 10 may be made of any material as long as it functions as an electrode. For example, when the organic EL display device of the present invention is a bottom-emission organic EL display device, a layer made of aluminum is preferably used as the second electrode 10 because of its excellent light reflectivity. When the organic EL display device is a top-emission organic EL display device, a silver alloy such as silver / magnesium is preferably used because of its excellent light transmittance. The second electrode 10 can be obtained by forming a film over the entire surface using a sputtering method.

[0162] The light extraction direction of the organic EL display device of the present invention is not particularly limited, and the organic EL display device may be a bottom-emission type organic EL display device in which the emitted light emitted from the light-emitting pixel 9 is extracted to the substrate side through the substrate 6, or a top-emission type organic EL display device in which the emitted light is extracted to the opposite side of the substrate 6 through the second electrode 10.

[0163] The substrate 6 can be a substrate made of rigid glass or a substrate made of flexible polyimide resin. Examples of glass include OA-10G and OA-11 (both manufactured by Nippon Electric Glass Co., Ltd.) and AN-100 (manufactured by Asahi Glass Co., Ltd.). Examples of polyimide resin substrates include substrates obtained by applying a solution containing polyamic acid to the surface of a temporary support, followed by heat treatment at 250 to 400°C to imidize the polyamic acid and convert it into a polyimide resin, and then peeling off the temporary support using a laser or the like. The polyamic acid used in this case can be synthesized by reacting a tetracarboxylic dianhydride and a diamine compound in an amide solvent such as N-methyl-2-pyrrolidone. Among these, polyamic acid having residues of an aromatic tetracarboxylic dianhydride and an aromatic diamine compound is preferred due to its low coefficient of linear thermal expansion and excellent dimensional stability. A specific example is polyamic acid having residues of 3,3',4,4'-biphenyltetracarboxylic dianhydride and p-phenylenediamine.

[0164] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to these embodiments.

[0165] [Evaluation Method] (1) Evaluation of Halftone Processability (Exposure Sensitivity, Residue) A silver alloy film (an alloy consisting of 99.00 mass % silver and 1.00 mass % copper) was formed on the entire surface of an alkali-free glass substrate measuring 150 mm long x 150 mm wide by a sputtering method. An ITO film was then formed on the entire surface by a sputtering method, thereby obtaining a glass substrate having a silver alloy film / ITO film on the entire surface of the alkali-free glass substrate.

[0166] The positive-type photosensitive pigment compositions obtained in each Example and Comparative Example were applied to the ITO surface of a glass substrate having a silver alloy film / ITO film using a spin coater, adjusting the rotation speed so that the film thickness was 4.5±0.2 μm. The applied film was then prebaked on a hot plate at 110° C. under atmospheric pressure for 120 seconds to obtain a prebaked film. The film thickness was measured using a stylus film thickness measuring device (Tokyo Seimitsu Co., Ltd.; Surfcom).

[0167] The obtained prebaked film was exposed to 40 to 300 mJ / cm using a mask aligner (mixed g, h, and i rays of an ultra-high pressure mercury lamp) through a positive halftone exposure mask (a mask in which 220 fully transparent square portions of 20.0 μm in length and 20.0 μm in width are arranged, and which is designed so that the exposure amount in the semi-transparent portions is 15% when the exposure amount in the fully transparent portions is 100% and the exposure amount in the shielding portions is 0%). 2 The pattern exposure was performed by changing the exposure dose stepwise in 10 mJ increments within the range of 10 mJ (i-line equivalent value) to obtain an exposed film having exposed, semi-exposed, and unexposed areas within the surface. The pattern exposure was performed by contacting a positive half-tone exposure mask with the surface of the prebaked film.

[0168] Next, in the development step, the substrate was developed using a small photolithography developing device (AD-1200; manufactured by Takizawa Sangyo Co., Ltd.) and a 2.38% by weight aqueous solution of tetramethylammonium hydroxide as an alkaline developer, using a paddle system. The paddle system, as used herein, refers to a method in which the alkaline developer is shower-applied to the surface of the exposed film for 10 seconds, followed by allowing the film to stand for a predetermined development time. The development time was within the range of 60 to 120 seconds, and was determined as the time required for the film thickness of the unexposed portion obtained after development to decrease by 1.0±0.1 μm from the film thickness of the prebaked film. The substrate was then rinsed with deionized water for 60 seconds using a shower system, and then dried by idling at 1000 rpm for 30 seconds, yielding a developed film-formed substrate having a developed film with a step (thick film portion in the unexposed portion and thin film portion in the partially exposed portion).

[0169] Next, as a curing step, the developed film was heated in air at 250°C for 1 hour using a high-temperature inert gas oven (INH-9CD-S; manufactured by Koyo Thermo Systems Co., Ltd.), to obtain a substrate for evaluating halftone processability, which was provided with a pixel dividing layer having a step in which the film thickness of the thick film portion was 3.0±0.2 μm and the film thickness of the thin film portion was 1.5±0.2 μm.

[0170] The obtained halftone processability evaluation substrate was used to observe the thin film portion of the pixel division layer using an FPD inspection microscope (MX-61L; manufactured by Olympus Corporation), and the minimum required exposure dose (mJ / cm) was determined when openings were made so that the average opening width of 10 openings in each exposure dose region was within the range of 20.0±0.1 μm. 2 The smaller the value, the better the exposure sensitivity. 2 When exposed to a light source with an aperture of 20.0±0.1 μm, or when exposed to a light source with an aperture of 300 mJ / cm 2 When the opening did not fall within the range of 20.0±0.1 μm even when exposed to light at 40 mJ / cm, it was judged that halftone processing was not possible. Evaluation was based on the following criteria, with A to C being considered as pass and D being considered as fail. A: Exposure sensitivity was 40 mJ / cm 2 Above, 100mJ / cm 2 B: Exposure sensitivity is less than 100 mJ / cm 2 Above, 200mJ / cm 2 C: Exposure sensitivity is less than 200 mJ / cm 2 Above, 300mJ / cm 2 D: Halftone processing is not possible.

[0171] Next, the positive photosensitive pigment compositions that were capable of halftone processing were evaluated for the amount of exposure light used as the exposure sensitivity, with respect to pigment residues in the openings (residues with a size of 0.1 to 3.0 μm resulting from re-adhering to the pattern openings of insoluble pigment particles in the film that had dissolved in the development step), residues at the opening edges (residues that remained undissolved at the opening edges), and minute residues in the openings (residues with a size of less than 0.1 μm).

[0172] (Evaluation of pigment residue) The presence or absence of pigment residue in 20 openings randomly selected from an array of 220 20.0 × 20.0 μm openings was observed using an FPD inspection microscope (MX-61L; manufactured by Olympus Corporation). The number of 0.1 to 3.0 μm pigment residues in the openings was measured, and the average of the 20 locations was taken as the number of pigment residues and evaluated based on the following criteria: A to C were rated as pass, and D and E were rated as fail. A: 0 pigment residues B: Less than 5 pigment residues C: 5 to less than 10 pigment residues D: 10 to less than 20 pigment residues E: 20 or more pigment residues.

[0173] (Evaluation of residue at opening edge) The undissolved residue at the edge of the opening measuring 20.0 × 20.0 μm was observed using an FPD inspection microscope (MX-61L; manufactured by Olympus Corporation) and a scanning electron microscope (SEM). The severity of the residue was evaluated based on the following criteria, with A, B, and C being considered acceptable, and D being considered unacceptable. A: Residue that cannot be confirmed in an SEM photograph at a magnification of 30,000 times. B: Residue that cannot be confirmed in an SEM photograph at a magnification of 5,000 times but can be confirmed in an SEM photograph at a magnification of 30,000 times. C: Residue that cannot be confirmed in an FPD inspection microscope at a magnification of 100 times but can be confirmed in an SEM photograph at a magnification of 5,000 times. D: Residue that can be confirmed in an FPD inspection microscope at a magnification of 100 times.

[0174] (Evaluation of Microresidue) The presence or absence of microresidues in 20 openings randomly selected from an array of 220 20.0 × 20.0 μm openings was observed using a scanning electron microscope (SEM). The number of microresidues less than 0.1 μm in the openings was measured, and the average of the 20 locations was taken as the number of microresidues and evaluated based on the following criteria: A to C were considered pass, and D and E were considered fail. A: 0 microresidues B: 1 or more but less than 10 microresidues C: 10 or more but less than 20 microresidues D: 20 or more but less than 30 microresidues E: 30 or more microresidues

[0175] (2) Preparation of Substrate for Evaluating Optical Properties Each of the positive photosensitive pigment compositions obtained in each of the Examples and Comparative Examples was applied to the surface of a transparent glass substrate ("Tempax" manufactured by AGC Technoglass Co., Ltd.) using a spin coater, adjusting the rotation speed so that the final cured film had a thickness of 1.5 μm, to obtain a coating film.

[0176] The coating film was prebaked at 110° C. for 120 seconds under atmospheric pressure using a hot plate (SCW-636; manufactured by Dainippon Screen Mfg. Co., Ltd.) to obtain a prebaked film.

[0177] Using a double-sided alignment single-sided exposure device, the entire surface of the prebaked film was irradiated with mixed rays of g, h, and i from an ultra-high pressure mercury lamp at an exposure amount equivalent to 15% of the exposure sensitivity (required minimum exposure amount) determined by the above-mentioned method, to obtain an exposed film.

[0178] The coating was developed, rinsed and dried in the same manner as in the evaluation of exposure sensitivity, to obtain a solid developed film.

[0179] The developed film was heated in air at 250°C for 1 hour using a high-temperature inert gas oven (INH-9CD-S; manufactured by Koyo Thermo Systems Co., Ltd.) to obtain a substrate for evaluating optical properties having a solid cured product with a film thickness of 1.5 µm.

[0180] (3) Evaluation of Light-Shielding Properties (OD / μm) of Cured Products For substrates for evaluating optical properties on which a 1.5 μm-thick cured film was formed using the positive photosensitive pigment compositions 1 to 23 obtained in each Example and Comparative Example, the total optical density (Total OD value) was measured at three locations on the film surface using an optical densitometer (X-Rite 361T, manufactured by X-Rite Corporation) to calculate the average value. This value was then divided by 1.5, and the resulting value was rounded to one decimal place to represent the OD value (OD / μm) per 1.0 μm of cured film thickness. The evaluation was based on the criterion that the higher the OD / μm value, the better the cured film, with higher light-shielding properties. The OD value of a transparent glass substrate ("Tempax") without a cured film formed thereon was separately measured and found to be 0.00. Therefore, the OD value of the substrate for evaluating optical properties was regarded as the OD value of the cured film. The thickness of the cured film was measured at three locations on the surface using a stylus film thickness measuring device (Tokyo Seimitsu Co., Ltd.; Surfcom), and the average value was rounded off to one decimal place to obtain a value up to one decimal place.

[0181] (4) Preparation of Organic EL Display Device for Evaluation A pixel dividing layer made of a cured product of a positive photosensitive pigment composition and an organic EL display device having the pixel dividing layer were prepared by the following method.

[0182] FIG. 2 shows a manufacturing process of an organic EL display device, including a process of forming a pixel dividing layer.

[0183] A silver alloy (an alloy consisting of 99.00% by mass of silver and 1.00% by mass of copper) was formed on the entire surface of an alkali-free glass substrate 11 measuring 70 mm long and 70 mm wide by sputtering. Using an alkali-soluble novolac-based positive resist, the substrate was immersed in a silver alloy etching solution SEA-1 at a solution temperature of 30°C and etched to obtain a patterned silver alloy film 12 with a thickness of 50 nm. Furthermore, an ITO film (indium-tin oxide) was formed on the entire surface by sputtering. Using an alkali-soluble novolac-based positive resist, the substrate was immersed in a 5% by mass aqueous oxalic acid solution at a solution temperature of 50°C for 5 minutes, shower-washed with deionized water for 2 minutes, and then dried with an air blower to obtain a patterned ITO film 13 with a thickness of 10 nm. Through the above steps, a first electrode-forming substrate was obtained, comprising a first electrode formed on the surface of the alkali-free glass substrate, the first electrode consisting of a laminated pattern of a silver alloy film / ITO film.

[0184] The positive photosensitive pigment composition was applied to the surface of the first electrode-forming substrate using a spin coater, adjusting the rotation speed so that the final pixel division layer having a step had a thickness of 3.0±0.2 μm in the thick film portion and 1.5 μm±0.2 in the thin film portion, to obtain a coating film. The coating film was then pre-baked using a hot plate at 110°C under atmospheric pressure for 120 seconds to obtain a pre-baked film, and a positive half-tone exposure mask (a mask designed to arrange 220 fully transparent square portions, each 30.0 μm long and 30.0 μm wide, and to provide a semi-transparent portion with an exposure of 15% when the exposure amount in the fully transparent portion is 100% and the exposure amount in the shielding portion is 0%) was aligned using a near-infrared camera (light source wavelength: 800 nm). The pre-baked film was then pattern-exposed through the positive half-tone exposure mask at the minimum required exposure amount (exposure sensitivity) determined by the above-mentioned method to obtain an exposed film. The pattern exposure was performed by contacting a positive half-tone exposure mask with the surface of the prebaked film. The film was then developed, rinsed, and dried in the same manner as in the evaluation of exposure sensitivity, yielding a patterned developed film. The developed film was heated in air at 250°C for 1 hour using a high-temperature inert gas oven to obtain a pixel division layer-forming substrate having 220 openings and a stepped pixel division layer 14 within a 30 mm x 30 mm area in the center of the first electrode-forming substrate.

[0185] Next, the organic EL layer 15 including the light-emitting layer was formed in the opening of the pixel dividing layer 14 by vacuum deposition. -3 Under vapor deposition conditions of 0.1 Pa or less, while rotating the pixel division layer-forming substrate relative to the vapor deposition source, first, a compound (HT-1) represented by formula (25) was deposited to a thickness of 10 nm as a hole injection layer, and a compound (HT-2) represented by formula (26) was deposited to a thickness of 50 nm as a hole transport layer. Next, a compound (GH-1) represented by formula (27) was deposited to a thickness of 40 nm as a host material, and a compound (GD-1) represented by formula (28) was deposited to a thickness of 40 nm on the light-emitting layer. Next, a compound (ET-1) represented by formula (29) and a compound (LiQ) represented by formula (30) were deposited to a thickness of 40 nm as electron transport materials in a volume ratio of 1:1.

[0186]

[0187]

[0188] Each layer constituting the organic EL layer 15 is extremely thin compared to the pixel division layer described above, and a stylus-type film thickness measuring device cannot provide high measurement accuracy. Therefore, each layer was measured using a quartz crystal oscillator film thickness monitor, which is suitable for thin films of less than 100 nm, and the value obtained by rounding off the average value of three points on the surface to the first decimal place was used as the film thickness.

[0189] Next, a compound (LiQ) was deposited to a thickness of 2 nm, and then a silver / magnesium alloy (volume ratio 10:1) was deposited to a thickness of 150 nm to form a second electrode 16 .

[0190] Next, a cap-shaped glass plate was adhered and sealed using an epoxy resin adhesive in a low humidity / nitrogen atmosphere to obtain an organic EL display device with an array of green light-emitting pixels.

[0191] (5) Evaluation of dark spots (local non-luminous areas) in pixels of organic EL display devices having pixel dividing layers For the organic EL display devices obtained in Examples 1 to 17 and Comparative Examples 1 to 4, the organic EL display devices were driven at 10 mA / cm 2 hours after the start of driving. 2 The device was driven by a direct current (DC) to emit light, and pixel portions formed within an area measuring 30 mm long x 30 mm wide were observed by enlarging 10 central pixel portions at 50x magnification on a monitor, and the number of locally non-emissive regions with a major axis of 0.1 μm or more and less than 15.0 μm in each opening was counted. The average number of locally non-emissive regions observed per opening was evaluated based on the following criteria, with A to C representing pass and D to E representing fail. A: No dark spots were observed. B: Fewer than 5 dark spots were observed. C: 5 to 10 dark spots were observed. D: 10 to 15 dark spots were observed. E: 15 or more dark spots were observed.

[0192] Synthesis Example 1 Synthesis of Hydroxyl Group-Containing Diamine Compound A 18.3 g (0.05 mol) of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane was dissolved in 100 mL of acetone and 17.4 g (0.3 mol) of propylene oxide and cooled to −15°C. A solution of 0.11 mol (20.4 g) of 3-nitrobenzoyl chloride dissolved in 100 mL of acetone was added dropwise to the solution. After the addition was completed, the reaction was allowed to proceed at −15°C for 4 hours and then returned to room temperature. The precipitated white solid was filtered and dried in vacuo at 50°C. 30 g of the solid was placed in a 300 mL stainless steel autoclave and dispersed in 250 mL of methyl cellosolve, followed by the addition of 2 g of 5% palladium-carbon. Hydrogen was introduced into the autoclave via a balloon, and the reduction reaction was carried out at room temperature. After approximately 2 hours, the reaction was terminated by confirming that the balloon was no longer deflating. After the reaction was completed, the catalyst palladium compound was removed by filtration, and the mixture was concentrated by a rotary evaporator to obtain a hydroxyl group-containing diamine compound A represented by formula (31).

[0193]

[0194] Synthesis Example 2: Synthesis of Polyimide Precursor (b-1) Under a dry nitrogen stream, 31.0 g (0.10 mol) of 3,3',4,4'-diphenylethertetracarboxylic acid dianhydride was dissolved in 500 g of NMP. To this solution, 45.35 g (0.075 mol) of hydroxyl group-containing diamine compound A and 1.24 g (0.005 mol) of 1,3-bis(3-aminopropyl)tetramethyldisiloxane were added along with 50 g of NMP, and the mixture was allowed to react at 20°C for 1 hour, followed by 2 hours at 50°C. 4.36 g (0.04 mol) of 4-aminophenol was added as an end-capping agent along with 5 g of NMP to terminate the reaction. Subsequently, 28.6 g (0.24 mol) of N,N-dimethylformamide dimethyl acetal (50 g) was added, and the mixture was stirred at 50°C for 3 hours. After stirring, the solution was cooled to room temperature and then poured into 3 L of water to obtain a white precipitate. The above procedure was repeated five times, and the resulting white precipitate was collected as a filter cake, washed five times with water, and then dried in a vacuum dryer at 80°C for 24 hours to obtain a polyimide precursor (b-1), which is an alkali-soluble resin (b). The weight-average molecular weight (Mw) of the polyimide precursor (b-1) was 25,000, and the amine value was 1.0 mgKOH / g.

[0195] Synthesis Example 3 Synthesis of Quinone Diazide Compound (d-1) Under a dry nitrogen stream, 21.22 g (0.05 mol) of TrisP-PA (manufactured by Honshu Chemical Industry Co., Ltd.) and 36.27 g (0.135 mol) of 5-naphthoquinone diazide sulfonyl chloride were dissolved in 450 g of 1,4-dioxane and the solution was allowed to cool to room temperature. To this solution, a solution of 15.18 g of triethylamine dissolved in 50 g of 1,4-dioxane was added dropwise while adjusting the system temperature to 35°C or below. After the addition, the mixture was stirred at 30°C for 2 hours. The triethylamine salt was filtered, and the filtrate was poured into water. The resulting precipitate was then filtered and collected. This precipitate was dried in a vacuum dryer to obtain quinone diazide compound (d-1) represented by formula (32), which is a photoacid generator (d).

[0196]

[0197] In formula (32), * represents the bonding site with the oxygen atom.

[0198] Synthesis Example 4 Synthesis of quinone diazide compound (d-2) A quinone diazide compound (d-2) represented by formula (33), which is a photoacid generator (d), was obtained by the same method as in Synthesis Example 3, except that 36.27 g (0.135 mol) of 4-naphthoquinone diazide sulfonyl chloride was used instead of 36.27 g (0.135 mol) of 5-naphthoquinone diazide sulfonyl chloride.

[0199]

[0200] In formula (33), * represents the bonding site with the oxygen atom.

[0201] [Production Example 1] Production of Perylene Pigment (a-1) To 2,648.16 g of phenol melted at 70°C, 588.48 g (1.50 mol) of perylene-3,4,9,10-tetracarboxylic dianhydride, 408.60 g (3.00 mol) of 4,5-dimethyl-1,2-phenylenediamine, and 64.61 g of piperazine were added. While stirring this mixture, the liquid temperature was raised to 170°C. Next, stirring was carried out at 170°C for 8 hours to allow the reaction to proceed sufficiently, and then the generated water was distilled off as an azeotrope with phenol. Next, the mixture was cooled to 130°C, and 500 g of ethanol was added in 50 g increments. After stirring at 60°C for 1 hour, the reaction product was filtered off. The filtrate was washed with ethanol until transparent, then washed with water, and dried under reduced pressure at 80°C for 24 hours to obtain Pigment Crude 1. Next, physical pulverization treatment was carried out by solvent salt milling according to the following procedure.

[0202] 500.00 g of Pigment Crude 1, 2.5 kg of grinding agent (sodium chloride particles with an average primary particle size of 0.5 μm that had been heat-treated at 230°C for 1 hour to reduce the moisture content to 0.1% by mass), and 250.00 g of dipropylene glycol were mixed and charged into a stainless steel 1-gallon kneader (manufactured by Inoue Seisakusho) and kneaded at 90°C for 10 hours. This kneaded mixture was added to 5 L of warm water and stirred for 1 hour while maintaining the temperature at 70°C to form a slurry. The mixture was then filtered and repeatedly washed with water until the chloride ion content, as determined by ion chromatography, was 50 ppm by mass or less, and the grinding agent and dipropylene glycol were removed. The mixture was then dried in an oven at 100°C under atmospheric pressure / air for 6 hours, after which the dried aggregates were deflocculated in a ball mill to obtain a perylene pigment (a-1) consisting of an isomer mixture of the compound represented by formula (34) and the compound represented by formula (35).

[0203]

[0204] The perylene pigment (a-1) is pigment (a), and has an average primary particle size of 26 nm, a maximum primary particle size of 110 nm, and an average aspect ratio of 1.1. The chemical structure of the perylene pigment (a-1) was analyzed using MALDI-TOF MS.

[0205] [Production Example 2] Production of dioxazine pigment (a-2) 1000.00 g of "Cromophtal" (registered trademark) Violet D5700 (manufactured by BASF: C.I. Pigment Violet 37) was heated in an oven at 200°C under atmospheric pressure / air for 1 hour, then cooled to room temperature, and dried and agglomerated was deaggregated in a ball mill to obtain dioxazine pigment 1. Next, a micronization treatment was carried out by solvent salt milling according to the following procedure.

[0206] 500.00 g of dioxazine pigment 1, 2.5 kg of grinding agent (sodium chloride particles with an average primary particle size of 0.5 μm that had been heat-treated at 230°C for 1 hour to reduce the moisture content to 0.1% by mass), and 250.00 g of dipropylene glycol were mixed and charged into a stainless steel 1-gallon kneader (manufactured by Inoue Seisakusho) and kneaded at 90°C for 5 hours to obtain a dark purple kneaded product. This kneaded product was added to 5 L of warm water and stirred for 1 hour while maintaining the temperature at 70°C to form a slurry. The grinding agent and dipropylene glycol were removed by washing with deionized water and filtering three times. The mixture was then dried in an oven at 200°C under atmospheric pressure / air for 6 hours, and then pulverized in a ball mill to loosen the dried aggregates, obtaining dioxazine pigment (a-2) consisting of the compound represented by formula (36).

[0207]

[0208] The dioxazine pigment (a-2) was pigment (a), and had an average primary particle size of 30 nm and a maximum primary particle size of 110 nm.

[0209] Synthesis Example 5 Synthesis of Organic Dye Particles (f-1) 50.00 g of C.I. Pigment Red 178 was dissolved in 500.00 g of 80% by mass concentrated sulfuric acid, heated, and stirred at a liquid temperature of 70°C for 6 hours to allow a sulfonation reaction to proceed. The resulting mixture was then poured into 5 kg of ice water to obtain a slurry containing a precipitate, which was then filtered. The filtered residue was then washed with ethanol, and repeatedly washed with water until the residual amount of sulfate ions fell below 50 ppm by mass, and dried at 80°C under reduced pressure for 24 hours. Furthermore, the resulting mixture was subjected to a dry grinding process using a fine grinder ("Nano Jetmizer" manufactured by Aisin Nano Technologies Co., Ltd.), and then passed through a stainless steel sieve filter (opening diameter 50 μm) to remove coarse particles, thereby obtaining organic dye particles (f-1). The organic dye particles (f-1) are organic dye particles (f) and are a mixture of a compound represented by formula (37), a compound represented by formula (38), and a compound represented by formula (39) in a mass ratio of 25:65:10.

[0210]

[0211] The chemical structure of the organic dye particles (f-1) was analyzed using MALDI-TOF MS, and the mass ratio of the compounds constituting the organic dye particles (f-1) was analyzed using LC-MS.

[0212] Preparation Example 1 Preparation of Pigment Dispersion Liquid A 60 g of polyimide precursor (b-1) as alkali-soluble resin (b) was added to 900 g of a mixed solvent (PGME, ethyl lactate, and γ-butyrolactone in a mass ratio of 50:40:10) as solvent (e), and the mixture was stirred for 30 minutes to dissolve. Furthermore, 10 g of pigment dispersant (f-1) as organic pigment particles (f) was added, and the mixture was stirred for 30 minutes. Next, 9 g of perylene pigment (a-1) and 21 g of dioxazine pigment (a-2) as pigment (a) were added, and the mixture was stirred for 30 minutes to obtain a preliminary stirred liquid. The pre-stirred liquid was then sent to a vertical bead mill, "Ultra Apex Mill Advance (registered trademark)" manufactured by Hiroshima Metal & Machinery Co., Ltd., whose vessel was filled with 0.05 mmφ zirconia beads ("Treceram (registered trademark)" manufactured by Toray Industries, Inc.) at a filling rate of 75% by volume, and subjected to wet media dispersion treatment using a circulation system at a peripheral speed of 10 m / s for 5 hours, yielding a pigment dispersion with a solids content of 10.00% by mass. The first filtration was performed using a 0.8 μm diameter filter, and then a second filtration was performed using a 0.2 μm diameter filter. No change in the solids content measured to two decimal places before and after filtration was observed, and a pigment dispersion A with a solids content of 10.00% by mass was obtained, with a mass ratio of pigment (a):organic pigment particles (f):(b) resin of 100:33:200. The blending masses of each raw material are shown in Table 1.

[0213] [Preparation Examples 2 to 5] Preparation of Pigment Dispersions B to E Pigment dispersions B to E were obtained in the same manner as in Preparation Example 1, except that 30 g each of a dioxazine pigment (a-2), a perylene pigment (a-1), a lactam organic black pigment "Irgaphor Black" (registered trademark) S0100CF (manufactured by BASF) (a'-3), and carbon black (a'-4) were used as the pigment (a) or a substitute thereof, in the correspondence shown in Table 1. The blend masses of each raw material are shown in Table 1.

[0214]

[0215] The names of the compounds used in each of the Examples and Comparative Examples are shown below. (c-1): 4,4',4''-trihydroxytriphenylmethane (molecular weight 292, alkyl group carbon number 1) (c-2): 4-hydroxybenzoic acid propyl (molecular weight 180, alkyl group carbon number 3) (c-3): propyl gallate (molecular weight 212, alkyl group carbon number 3) (c1-1): 2-hydroxy-4-octyloxybenzophenone (molecular weight 326, alkyl group carbon number 8) (c1-2): 4-dodecylphenol (molecular weight 262, alkyl group carbon number 12) (c1-3): 4-hydroxybenzoic acid octyl (molecular weight 250, alkyl group carbon number 8) (c1-4): octyl gallate (molecular weight 282, alkyl group carbon number 8) (c1-5): hexadecyl gallate (molecular weight 394, alkyl group carbon number 16) (c2-1): pyrogallol (c2-2): 1,2,4-trihydroxybenzene (c2-3): 2,4,5-trihydroxybenzaldehyde (c'-1): 4-n-octyloxybenzoic acid (molecular weight 250, alkyl group carbon number 8).

[0216] Example 1 To 17.95 g of PGME as a solvent (e), 0.40 g of polyimide precursor (b-1) as an alkali-soluble resin (b), 0.20 g of 4,4′,4″-trihydroxytriphenylmethane (c-1) as a compound (c), 0.50 g of 2-hydroxy-4-octyloxybenzophenone (c1-1) as a compound (c1), 0.50 g of quinone diazide compound (d-1) and 0.40 g of quinone diazide compound (d-2) as photoacid generators (d), and 0.05 g of a PGME solution with a solids content of 5% by mass of BYK-333 (manufactured by BYK Japan KK) as a leveling agent were added, and the mixture was stirred for 30 minutes to dissolve. Further, 30.0 g of Pigment Dispersion A was added, and the mixture was stirred for 30 minutes to prepare a positive-type photosensitive pigment composition 1 having a solid content of 10.0% by mass. Table 2 shows the blending masses of each raw material.

[0217] After preparation, positive photosensitive pigment composition 1 was added to a 50 mL light-shielding glass bottle, sealed, and stored in a cool, dark place maintained at -20±1°C under atmospheric pressure and protected from light. After storage for one day, the bottle was removed from the cool, dark place and allowed to cool to room temperature (23°C), and then used for various evaluations and for producing organic EL display devices. The evaluation results are shown in Table 2.

[0218] [Examples 2 to 8] Positive photosensitive pigment compositions 2 to 8 were prepared in the amounts shown in Table 2 by replacing compound (c1-1) with compounds (c1-2) to (c1-5) and compounds (c2-1) to (c2-2) in the amounts shown in Table 2. The evaluation results are shown in Table 2.

[0219]

[0220] [Examples 9 and 10] Positive photosensitive pigment compositions were prepared using the formulations and blending amounts shown in Table 3. Otherwise, positive photosensitive pigment compositions 9 to 10 were obtained in the same manner as in Example 1. The pigment dispersion liquid was changed between these examples. The evaluation results are shown in Table 3.

[0221] [Examples 11 and 12] The amount of pigment dispersion A was increased, and positive photosensitive pigment compositions were prepared in the blending amounts shown in Table 3. Otherwise, positive photosensitive pigment compositions 11 and 12 were obtained in the same manner as in Example 1. The evaluation results are shown in Table 3.

[0222]

[0223] [Examples 13 to 17] Positive photosensitive pigment compositions were prepared according to the formulations and blending amounts shown in Table 4. Otherwise, positive photosensitive pigment compositions 19 to 23 were obtained in the same manner as in Example 1. The evaluation results are shown in Table 4.

[0224]

[0225] [Comparative Example 1] Compound (c1-1) was replaced with an increased amount of compound (c-1), and a positive photosensitive pigment composition was prepared in the blending amounts shown in Table 5. Otherwise, the same procedure as in Example 1 was carried out to obtain positive photosensitive pigment composition 13. The evaluation results are shown in Table 5.

[0226] [Comparative Examples 2 to 4] Compounds (c'-1), (c-2), and (c-3) were used instead of compound (c1-1) to prepare positive photosensitive pigment compositions in the amounts shown in Table 5. Otherwise, positive photosensitive pigment compositions 14 to 16 were obtained in the same manner as in Example 1. The evaluation results are shown in Table 5.

[0227] [Comparative Examples 5 and 6] Using pigment dispersion D or E instead of pigment dispersion A, positive photosensitive pigment compositions were prepared in the blending amounts shown in Table 5. Otherwise, the same procedure as in Example 1 was repeated to obtain positive photosensitive pigment compositions 17 and 18. The evaluation results are shown in Table 5. However, because halftone processing became difficult, it was not possible to evaluate residues and dark spots in the pixels of the organic EL display device.

[0228]

[0229] From the above results, it can be seen that the positive photosensitive pigment compositions of Examples 1 to 17 are free from redeposition residue and have excellent halftone processability compared to the positive photosensitive pigment compositions of Comparative Examples 1 to 4.

[0230] In particular, in the cases of Examples 11 and 12, which form pixel division layers with high light-blocking properties, with an OD value of 1.3 or 1.5 per 1.0 μm of cured film thickness, by containing compound (c1), excellent halftone processability with no pigment residue was obtained, similar to Examples 1 to 10 and 13 to 17, which form cured film with an OD value of 1.0 per 1.0 μm of cured film thickness.

[0231] Furthermore, Example 6, which contains compound (c2), has less residue at the edge of the opening and exhibits excellent halftone processability compared to Examples 1 to 5. Furthermore, Examples 7 to 12, which have a more preferable ratio of compound (c1) to compound (c2), exhibit even less edge residue and exhibit even more excellent halftone processability compared to Example 6.

[0232] Furthermore, in Examples 7 to 12 and 15 to 16, in which the compound (c2) represented by formula (40) was used and the quantitative ratio of the compound (c1) to the compound (c2) was more preferable, excellent halftone processability was obtained with no minute residue of less than 0.1 in the openings.

[0233] Furthermore, the organic EL display devices using the positive photosensitive pigment compositions of Examples 1 to 18 are superior to the organic EL display devices using the positive photosensitive pigment compositions of Comparative Examples 1 to 5 in that they have fewer dark spots in the pixels, and Examples 5 to 17 are particularly superior.

[0234] Therefore, it is clear that the positive photosensitive pigment composition of the present invention and an organic EL display device comprising a cured product of the positive photosensitive pigment composition are useful.

[0235] The positive photosensitive pigment composition of the present invention can be preferably used in applications requiring the formation of a high-definition cured film with stable high exposure sensitivity, such as a material for forming pixel dividing layers in organic EL display devices, TFT planarizing layers in organic EL display devices, partition walls in quantum dot organic EL display devices (QD-OLED), planarizing layers in micro LED displays, black matrices in liquid crystal display devices, black column spacers in liquid crystal display devices, near-infrared-transmitting visible light-shielding films in solid-state imaging devices, black bezels in display devices, etc. In particular, the composition can be particularly preferably used as a material for forming pixel dividing layers provided in organic EL display devices equipped with a bendable flexible display.

[0236] 1: TFT 2: Wiring 3: TFT insulating layer 4: Planarization layer 5: First electrode 6: Substrate 7: Contact hole 8: Pixel dividing layer 9: Light-emitting pixel 10: Second electrode 11: Alkali-free glass substrate 12: Silver alloy film 13: ITO film 14: Pixel dividing layer 15: Organic EL layer 16: Second electrode

Claims

1. A positive-type photosensitive pigment composition comprising a pigment (a), which is a dioxazine pigment and / or a perylene pigment having a benzimidazole skeleton, an alkali-soluble resin (b), a compound (c) having a phenolic hydroxyl group and a molecular weight of 1,000 or less, a photoacid generator (d) and a solvent (e), wherein the compound (c) contains a compound (c1) having an alkyl group having 5 to 20 carbon atoms.

2. The positive photosensitive pigment composition according to claim 1, further comprising organic pigment particles (f) having a sulfo group.

3. The positive photosensitive pigment composition according to claim 1 or 2, wherein the content of the pigment (a) is 10 to 30 mass % relative to 100 mass % of the solid content of the positive photosensitive pigment composition.

4. The positive photosensitive pigment composition according to claim 1 or 2, wherein the compound (c1) contains a compound represented by formula (1). (In formula (1), R 1 represents -NH- or an oxygen atom. 2 R represents an alkyl group having 5 to 20 carbon atoms. 3 , R 4 , R 5 , R 6 and R 7 each independently represents a hydrogen atom, an alkyl group, or a hydroxyl group. 3 , R 4 , R 5 , R 6 and R 7 The total number of hydroxyl groups is 1 to 3.

5. The positive photosensitive pigment composition according to claim 1 or 2, wherein the compound (c1) contains a compound having an alkyl group having 12 to 18 carbon atoms.

6. The positive photosensitive pigment composition according to claim 1 or 2, wherein compound (c) contains a compound (c2) which does not have an alkyl group having 5 to 20 carbon atoms and has an aryl group substituted with three or more phenolic hydroxyl groups.

7. The positive photosensitive pigment composition according to claim 6, wherein the compound (c2) is a compound represented by formula (40). In formula (40), n 24 is 3 to 6.

8. The positive photosensitive pigment composition according to claim 6, wherein the content of compound (c1) in compound (c) is 15 to 70 mass %, and the content of compound (c2) in compound (c) is 30 to 85 mass %.

9. The positive photosensitive pigment composition according to claim 7, wherein the ratio mc1 / mc2 of the content (mass) mc1 of compound (c1) to the content (mass) mc2 of compound (c2) is 0.3 or more and less than 1.

0.

10. A cured product derived from the positive photosensitive pigment composition according to claim 1 or 2.

11. An organic EL display device comprising the cured product according to claim 10.

Citation Information

Patent Citations

  • Photosensitive resin composition for forming insulation film in organic el display element

    JP2016031788A

  • Photosensitive composition, color filter, and microlens derived therefrom

    JP2020515893A

  • Photosensitive resin composition, method for producing electrically conductive pattern, substrate, touch panel, and display

    WO2018061384A1

Cited By

  • Polyimide precursor composition, polyimide resin, wiring circuit board, and electronic device

    WO2026033922A1