Method for manufacturing laminate

The method of laminating a resin film on a substrate with controlled pressure and temperature ensures improved embeddability of the first cladding layer within through-holes, addressing optical losses and enhancing light propagation in opto-electrical composite substrates.

WO2024204344A1PCT designated stage expired Publication Date: 2024-10-03SUMITOMO BAKELITE CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012248
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional opto-electrical composite substrates face challenges in achieving sufficient embeddability of the first cladding layer within through-holes, leading to optical losses due to dents or voids, which affect light propagation.

Method used

A method involving a substrate with through-holes and a first cladding layer, where a resin film is placed on the substrate, and then laminated using a vacuum laminating device under controlled pressure and temperature, ensuring the resin layer fills at least 70% of the through-hole volume.

Benefits of technology

This method enhances embeddability, reducing optical losses by effectively filling the through-holes with the resin composition, thereby improving the light propagation efficiency of the opto-electrical composite substrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012248_03102024_PF_FP_ABST
    Figure JP2024012248_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a method for manufacturing a laminate that comprises: a substrate (110) having a through hole (140); and a first cladding layer (20) of an optical waveguide (100). The method comprises at least: a step (A) for preparing, on the substrate (110), a workpiece (400) on which is placed a resin film (300) comprising a resin layer (a) (310), made of a resin composition, for forming the first cladding layer (20); and a step (B) for laminating the first cladding layer (20) on the substrate (110) by heating and pressing the workpiece (400) under reduced pressure using a vacuum laminating device.
Need to check novelty before this filing date? Find Prior Art

Description

Manufacturing method of laminate

[0001] The present invention relates to a method for producing a laminate.

[0002] BACKGROUND ART In recent years, there has been a demand for components in information and communication devices that can realize more advanced information communication, such as larger information capacity and faster information communication speed, and an optoelectronic composite substrate has been considered as one such component.

[0003] The optical / electrical composite substrate may be, for example, a substrate on which an optical waveguide is provided. Techniques relating to the manufacturing method of an optical waveguide include those described in Patent Documents 1 to 3, for example.

[0004] Patent Document 1 describes a method for manufacturing an embedded polyimide optical waveguide, characterized in that an upper cladding layer is formed between an arbitrary substrate and a ridge-type waveguide, and the upper cladding layer has the same heat resistance as the substrate and a lower refractive index than the core, and the method for manufacturing a polyimide optical waveguide described in Patent Document 1 states that a polyimide optical waveguide can be manufactured on an arbitrary substrate.

[0005] Patent Document 2 describes an opto-electrical hybrid board including a flexible circuit board having electrical wiring with mounting pads formed on the surface of an insulating layer, a device mounted on the mounting pads, and an optical waveguide laminated on the back surface of the insulating layer, wherein the flexible circuit board is a flexible double-sided circuit board having electrical wiring also formed on the back surface of the insulating layer, and a metal reinforcing layer is plated on at least a portion of the electrical wiring on the back surface corresponding to the mounting pads, and the optical waveguide is in contact with the metal reinforcing layer. Patent Document 2 describes an opto-electrical hybrid board in which the metal reinforcing layer is adhered to the insulating layer of the flexible circuit board without an adhesive layer, and the metal reinforcing layer prevents deformation due to a pressure load during device mounting, thereby providing an opto-electrical hybrid board in which the device is properly mounted.

[0006] Patent Document 2 describes preparing a substrate having copper foil 21 formed on both sides of an insulating layer 1 made of a resin such as polyimide, and forming through holes 1a and via holes 1b for optical paths in the substrate (see paragraph 0023 of Patent Document 2). Patent Document 2 also describes a flexible double-sided circuit board E having a metal reinforcing layer M formed thereon (see paragraph 0028 of Patent Document 2). The flexible double-sided circuit board E includes the substrate. Patent Document 2 also describes forming an undercladding layer 6 on the back side of the flexible double-sided circuit board E in contact with the metal reinforcing layer M covering the electrical wiring 2B on the back side. Examples of molding materials for the undercladding layer 6 include photosensitive resins and thermosetting resins (see paragraph 0029 of Patent Document 2). Figures 4 to 6 of Patent Document 2 show that the molding material for the undercladding layer 6 is filled into recesses formed in the flexible double-sided circuit board E having the metal reinforcing layer M formed thereon.

[0007] Patent Document 3 describes an optoelectronic wiring board that is formed by integrating a rigid section in which conductor circuits and insulating layers are laminated on both sides of a substrate with one or more bendable flex sections, wherein the rigid section has external connection terminals formed therein for mounting optical elements and / or package substrates on which optical elements are mounted, and at least one of the flex sections has optical wiring formed therein. It is described that the optoelectronic wiring board in Patent Document 3 can suitably process large amounts of information and high-speed information processing without increasing the size of the wiring board.

[0008] Patent Document 3 describes that the rigid section has an optical signal transmitting region formed therein, and that the optical signal transmitting region is filled with a resin composition (see claims 4 and 5 of Patent Document 3). Patent Document 3 also describes that the optical signal transmitting region is formed so as to penetrate all of the substrates and insulating layers that make up the rigid section (see claim 6 of Patent Document 3).

[0009] Furthermore, Patent Document 3 describes a substrate 221 consisting of an optical waveguide film 250 and a surrounding resin layer (insulating layer) 221a, and describes that the resin layer 221a constitutes part of the optical signal transmitting regions 242a, 242b (see paragraph 0033 of Patent Document 3).

[0010] JP 2000-321455 A JP 2014-238455 A JP 2006-140233 A

[0011] In conventional technology relating to optoelectronic composite substrates, there are known optoelectronic composite substrates in which recesses or through holes formed in a substrate are filled with a resin composition (see, in particular, Patent Documents 2 and 3).

[0012] For example, a manufacturing process for an optoelectronic composite substrate includes a process of integrating a substrate having a through-hole with a film for an optical waveguide clad. In this process, the through-hole formed in the substrate needs to be filled with the optical waveguide clad (hereinafter, "embeddability" refers to the property of how much the optical waveguide clad can be embedded in the through-hole).

[0013] The present invention has been made in view of the above circumstances, and provides a method for producing a laminate that can provide an optoelectronic composite substrate with improved embeddability.

[0014] According to the present invention, there is provided the following method for producing a laminate.

[0015] [1] A method for manufacturing a laminate including a substrate having a through hole and a first clad layer of an optical waveguide, the method comprising at least the steps of: (A) preparing a workpiece including a resin film placed on the substrate, the resin film including a resin layer (a) made of a resin composition for forming the first clad layer; and (B) laminating the first clad layer onto the substrate by heating and pressing the workpiece under reduced pressure using a vacuum laminator. [2] The method for manufacturing the laminate according to [1], wherein T / R is 0.10 or greater, where T [μm] is the thickness of the substrate and R [μm] is the diameter of the through hole. [3] The method for manufacturing the laminate according to [1] or [2], wherein the diameter of the through hole is 10 μm or greater and 1000 μm or less. [4] The method for manufacturing a laminate according to any of [1] to [3], wherein the thickness of the substrate is 10 μm or greater and 1000 μm or less. [5] The method for producing a laminate according to any one of [1] to [4], wherein the resin layer (a) has a thickness of 10 μm or more and 300 μm or less. [6] The method for producing a laminate according to any one of [1] to [5], wherein the resin layer (a) has a thickness smaller than the thickness of the substrate. [7] The resin layer (a) has a complex viscosity η* at 100°C of 1.0 x 10 when the complex viscosity is measured by a melt viscoelasticity test under the conditions of a measurement frequency of 10 rad / sec, a temperature range of 23°C to 200°C, and a heating rate of 3°C / min. 3 Pa・s or more 1.0×10 7[8] The method for producing a laminate according to any one of [1] to [6], wherein the viscosity of the laminate is 1 Pa s or less. [8] The method for producing a laminate according to any one of [1] to [7], wherein the resin layer (a) contains at least one selected from the group consisting of a polyimide resin, a compound having a cyclic ether structure, and a copolymer of a styrene-based monomer and a diene-based monomer. [9] The method for producing a laminate according to any one of [1] to [8], wherein in step (B), the work is heated to 80°C or higher and 190°C or lower and pressed.

[10] The method for producing a laminate according to any one of [1] to [9], wherein in step (B), the work is sandwiched between two press plates, and the work is heated and pressed.

[11] The method for producing a laminate according to

[10] , wherein in step (B), at least one of the two press plates contains rubber.

[12] The method for producing a laminate according to any one of [1] to

[11] , wherein in step (B), the degree of vacuum is 500 Pa or less.

[13] The method for producing a laminate according to any one of [1] to

[12] , wherein in step (B), the pressure when pressing the workpiece is 0.3 MPa or more and 10.0 MPa or less.

[14] The method for producing a laminate according to any one of [1] to

[13] , further comprising, after step (B), step (C) of sandwiching the workpiece between two press plates and heating and pressing the workpiece.

[15] The method for producing a laminate according to any one of [1] to

[14] , wherein, when the volume of the through hole in the laminate is 100 vol%, 70 vol% or more of the through hole is filled with a resin composition for forming the first clad layer.

[16] The method for producing a laminate according to any one of [1] to

[15] , wherein the laminate is an optical / electrical composite substrate further comprising a core layer and a second clad layer, in this order, on the first clad layer.

[0016] According to the present invention, it is possible to provide a method for manufacturing a laminate that can obtain an optoelectronic composite substrate with improved embeddability.

[0017] 1 is a cross-sectional view schematically showing an example of the structure of an optoelectronic composite substrate according to an embodiment of the present invention; 2 is a cross-sectional view schematically showing an example of the structure of a workpiece in step (A);

[0018] Hereinafter, embodiments of the present invention will be described with reference to the drawings. Numerical ranges "A to B" represent A or more and B or less unless otherwise specified.

[0019] FIG. 1 is a cross-sectional view schematically illustrating an example of the structure of an optoelectronic composite substrate according to this embodiment. Note that the diagram is a simplified view and does not correspond to the actual dimensional ratio. As shown in FIG. 1 , an optoelectronic composite substrate 200 includes an optical waveguide 100 provided on a substrate 110. The optical waveguide 100 includes a first cladding layer 20, a core layer 30, and a second cladding layer 40 stacked in this order. The optical waveguide 100 includes a mirror 50 on the light-emitting element side and a mirror 60 on the light-receiving element side. The substrate 110 has through-holes 140 (140a, 140b) (note that the through-hole 140 shown in FIG. 1 is filled with the first cladding layer 20). A light-emitting element 120 and a light-receiving element 130 are provided on the side of the substrate 110 opposite the optical waveguide 100 side.

[0020] The propagation path of light in the photoelectric composite substrate 200 will be specifically described using Figure 1. Light emitted from the light-emitting portion of the light-emitting element 120 passes through a through-hole 140a formed in the substrate 110, enters the mirror 50 on the light-emitting element side, and is transmitted through the core layer 30. After that, it enters the mirror 60 on the light-receiving element side, passes through a through-hole 140b formed in the substrate 110, and enters the light-receiving element 130. The arrows in Figure 1 are a schematic representation of the propagation of light.

[0021] The inventors have found through their studies that conventional methods for manufacturing an optical / electrical composite substrate fail to sufficiently embed the first clad layer in through holes formed in the substrate, resulting in the formation of depressions on the surface of the optical waveguide clad opposite the substrate side (i.e., the core layer side of the first clad layer) or voids in the through holes. The inventors have found that the through holes are a path for light propagation, and that when the above-mentioned depressions or voids occur in the optical / electrical composite substrate, optical loss occurs at the interfaces of the depressions or voids. The present invention has been made in view of the above circumstances, and provides a method for manufacturing a laminate that can obtain an optical / electrical composite substrate with improved embeddability.

[0022] The method for manufacturing a laminate of this embodiment is a method for manufacturing a laminate comprising a substrate having a through hole and a first clad layer of an optical waveguide, and comprises at least the steps of: (A) preparing a workpiece on which a resin film comprising a resin layer (a) made of a resin composition for forming the first clad layer is placed on the substrate; and (B) laminating the first clad layer onto the substrate by heating and pressing the workpiece under reduced pressure using a vacuum laminating device.

[0023] Each step of the method for producing a laminate according to this embodiment will now be described in detail.

[0024] [Step (A) of Preparing a Workpiece] The method for manufacturing a laminate of this embodiment includes step (A) of preparing a workpiece in which a resin film having a resin layer (a) made of a resin composition for forming a first clad layer is placed on a substrate.

[0025] 2 is a cross-sectional view showing a schematic example of the structure of the workpiece in step (A). Note that the drawing is a simplified view and does not correspond to the actual dimensional ratio. The workpiece 400 has a resin film 300 placed on a substrate 110, the resin film 300 including a resin layer (a) 310 made of a resin composition for forming a first clad layer. Here, a through hole 140 is formed in the substrate 110.

[0026] The resin film 300 may be a single-layer film composed of only the resin layer (a) 310, or may be a multi-layer film as shown in FIG. 2, but is preferably a film in which the resin layer (a) 310 and a base film 320 are laminated. When the resin film 300 includes the base film 320, the resin film 300 is easier to handle and contamination of the vacuum laminating device can be prevented. When the resin film 300 is a multi-layer film, the resin film 300 is placed on the substrate 110 so that the resin layer (a) 310 faces the substrate 110.

[0027] There are no particular limitations on the substrate 110 as long as it is a substrate having through holes. Examples of the substrate 110 include a printed circuit board and a flexible substrate, and the flexible substrate is preferred, and a flexible double-sided copper-clad laminate is more preferred.

[0028] The thickness of the substrate 110 is preferably 10 μm or more, more preferably 30 μm or more, even more preferably 40 μm or more, and even more preferably 45 μm or more, and from the viewpoint of miniaturizing the optoelectronic composite substrate, it is preferably 1000 μm or less, more preferably 800 μm or less, even more preferably 500 μm or less, even more preferably 300 μm or less, even more preferably 200 μm or less, even more preferably 100 μm or less, and even more preferably 80 μm or less.

[0029] The substrate 110 has at least one through hole 140, and may have one through hole 140 or may have two or more through holes 140. Specifically, for example, in the substrate 110 shown in Figures 1 and 2, the through hole 140 serves as a propagation path for light, and therefore the substrate 110 has a through hole 140a on the light-emitting element side and a through hole 140b on the light-receiving element side.

[0030] The diameter of the through-hole 140 is preferably 10 μm or more, more preferably 30 μm or more, even more preferably 50 μm or more, even more preferably 70 μm or more, even more preferably 90 μm or more, and is preferably 1000 μm or less, more preferably 800 μm or less, even more preferably 500 μm or less, even more preferably 400 μm or less, even more preferably 350 μm or less, even more preferably 140 μm or less. Here, when the substrate 110 has a plurality of through-holes 140, it is sufficient that the diameter of at least one of the through-holes 140 is within the above range.

[0031] When the thickness of the substrate 110 is T [μm] and the diameter of the through hole 140 is R [μm], T / R is preferably 0.10 or more, more preferably 0.13 or more, even more preferably 0.15 or more, even more preferably 0.20 or more, even more preferably 0.25 or more, even more preferably 0.27 or more, even more preferably 0.30 or more, even more preferably 0.35 or more, even more preferably 0.40 or more, even more preferably 0.45 or more, and even more preferably 0.60 or more. The upper limit is not particularly limited, but may be, for example, 2.00 or less, 1.50 or less, or 1.00 or less. Here, when the substrate 110 has multiple through holes 140, it is sufficient that the T / R of at least one of the through holes 140 is within the above range. In general, the larger the T / R, the more difficult it is to sufficiently fill the through holes with the first cladding layer. On the other hand, according to the method for manufacturing a laminate of this embodiment, even when T / R is large, it is possible to sufficiently fill the through-holes with the first cladding layer.

[0032] A preferred embodiment of the resin film 300 will be described later.

[0033] [Laminating Step (B)] The method for producing a laminate according to this embodiment includes a step (B) of laminating a first clad layer onto a substrate by heating and pressing a workpiece under reduced pressure using a vacuum laminating device. By heating and pressing the workpiece under reduced pressure, the substrate and the resin layer (a) can be laminated together. Because the resin layer (a) is made of a resin composition for forming the first clad layer, in other words, by heating and pressing the workpiece under reduced pressure, the substrate and the first clad layer can be laminated together.

[0034] In step (B), the workpiece is heated and pressed under reduced pressure. Here, "reduced pressure" means that the degree of vacuum is lower than atmospheric pressure (1013 hPa). In step (B), the degree of vacuum is preferably 500 Pa or less, more preferably 400 Pa or less, even more preferably 350 Pa or less, and even more preferably 320 Pa or less, from the viewpoint of further improving embeddability. The lower limit is not particularly limited, but may be, for example, 10 Pa or more, or 50 Pa or more.

[0035] In step (B), the pressure when pressing the workpiece is preferably 0.3 MPa or more, more preferably 0.5 MPa or more, even more preferably 1.0 MPa or more, even more preferably 1.3 MPa or more, even more preferably 2.0 MPa or more, even more preferably 3.0 MPa or more, even more preferably 4.0 MPa or more, from the viewpoint of further improving embeddability, and is preferably 10.0 MPa or less, more preferably 8.0 MPa or less, even more preferably 6.0 MPa or less, from the viewpoint of preventing damage to the substrate.

[0036] In step (B), the temperature of the workpiece when heated and pressed is preferably 80°C or higher, more preferably 90°C or higher, even more preferably 95°C or higher, from the viewpoint of further improving embeddability, and is preferably 190°C or lower, more preferably 180°C or lower, even more preferably 150°C or lower, and even more preferably 145°C or lower. Here, the temperature of the workpiece may be considered to be the same as the set press temperature of the vacuum laminator. This is because the workpiece is thin and is thought to reach the same temperature as the set press temperature within a few seconds of being placed in the vacuum laminator.

[0037] In step (B), the time for pressing the workpiece is preferably 30 seconds or more, more preferably 60 seconds or more, even more preferably 80 seconds or more, and even more preferably 100 seconds or more, from the viewpoint of further improving embeddability, and is preferably 210 seconds or less, more preferably 180 seconds or less, even more preferably 150 seconds or less, and even more preferably 130 seconds or less, from the viewpoint of further improving productivity.

[0038] In step (B), the method for heating and pressing the workpiece is not particularly limited, and may be a flat plate press or a roll press. In step (B), the method for heating and pressing the workpiece is preferably a flat plate press, in other words, preferably in step (B), the workpiece is sandwiched between two press plates, and the workpiece is heated and pressed.

[0039] In step (B), when the workpiece is sandwiched between two press plates and heated and pressed, it is preferable that at least one of the two press plates contains rubber, and it is preferable that both of the two press plates contain rubber. The rubber is not particularly limited, but examples include silicone rubber, fluororubber, and acrylic rubber. When the press plate has a two-layer or more structure, it is preferable that the surface of the press plate that contacts the workpiece contains rubber.

[0040] In step (B), the vacuum laminating device is not particularly limited, but for example, a rubber press laminator, a diaphragm laminator, etc. can be used, and a rubber press laminator is preferably used. Specific examples of rubber press laminators include CVP-600 (manufactured by Nikko Materials Co., Ltd.) and CVP-700 (manufactured by Nikko Materials Co., Ltd.). Examples of diaphragm laminators include CVP-300 (manufactured by Nikko Materials Co., Ltd.) and MVLP-500 / 600-IIA (manufactured by Meiki Seisakusho).

[0041] [Pressing Step (C)] The method for producing a laminate according to the present embodiment preferably further comprises, after step (B), step (C) of sandwiching the workpiece between two press plates and heating and pressing the workpiece. By further comprising step (C), it is possible to further improve embeddability, and more specifically, it is possible to suppress the occurrence of depressions on the surface of the first clad layer opposite to the substrate side.

[0042] The degree of vacuum in step (C) is not particularly limited, and the workpiece may be heated and pressed at normal pressure or may be heated and pressed under reduced pressure. When the workpiece is heated and pressed under reduced pressure in step (C), the preferred degree of vacuum is the same as the preferred degree of vacuum in step (B).

[0043] In step (C), the pressure when pressing the workpiece is preferably 0.3 MPa or more, more preferably 0.5 MPa or more, even more preferably 1.0 MPa or more, even more preferably 1.3 MPa or more, even more preferably 2.0 MPa or more, even more preferably 3.0 MPa or more, even more preferably 4.0 MPa or more, from the viewpoint of further improving embeddability, and is preferably 10.0 MPa or less, more preferably 8.0 MPa or less, even more preferably 6.0 MPa or less, from the viewpoint of preventing damage to the substrate.

[0044] In step (C), the temperature of the workpiece when heated and pressed is preferably 80°C or higher, more preferably 90°C or higher, even more preferably 95°C or higher, from the viewpoint of further improving embeddability, and is preferably 190°C or lower, more preferably 180°C or lower, even more preferably 150°C or lower, and even more preferably 145°C or lower. Here, the temperature of the workpiece may be considered to be the same as the set press temperature of the press device. This is because, due to the thin thickness of the workpiece, the temperature of the workpiece is considered to reach the same temperature as the set press temperature within a few seconds after being placed in the press device.

[0045] In step (C), the time for pressing the workpiece is preferably 5 seconds or more, more preferably 10 seconds or more, and even more preferably 20 seconds or more, from the viewpoint of further improving embeddability, and is preferably 100 seconds or less, more preferably 80 seconds or less, more preferably 60 seconds or less, and even more preferably 40 seconds or less, from the viewpoint of further improving productivity.

[0046] In step (C), the method for heating and pressing the workpiece is not particularly limited, and may be a flat plate press or a roll press. In step (C), the method for heating and pressing the workpiece is preferably a flat plate press, in other words, preferably in step (C), the workpiece is sandwiched between two press plates, and the workpiece is heated and pressed.

[0047] In step (C), the press device is not particularly limited, but from the viewpoint of further improving productivity, it is preferable that the vacuum laminator used in step (B) is a two-stage type and a flattening stage corresponding to the second stage is used. That is, when the vacuum laminator is a two-stage type, step (B) can be performed in a laminator corresponding to the first stage, and step (C) can be performed in a flattening stage corresponding to the second stage. After step (B), the workpiece can be removed from the vacuum laminator used in step (B), and step (C) can be performed using a press device different from that used in step (B).

[0048] [Other Steps] The method for producing a laminate according to the present embodiment may include steps other than step (A), step (B), and step (C). Examples of other steps include a step of laminating another layer after step (C).

[0049] [Laminate] The laminate obtained by the laminate manufacturing method of this embodiment includes a substrate having a through hole and a first clad layer of an optical waveguide. Here, in the laminate of this embodiment, the first clad layer of the optical waveguide is conceptually considered to include the resin layer (a). The laminate of this embodiment may further include other layers, and may be, for example, a laminate including a substrate, a first clad layer, and a base film in this order.

[0050] The laminate of this embodiment is preferably an optoelectronic composite substrate further comprising a core layer and a second clad layer on the first clad layer, in this order. That is, the optoelectronic composite substrate comprises a substrate, a first clad layer, a core layer, and a second clad layer, in this order. The optoelectronic composite substrate of this embodiment may further comprise a polyimide substrate on the surface of the second clad layer opposite to the core layer.

[0051] The optoelectronic composite substrate of this embodiment can be produced, for example, as follows. First, steps (A) and (B) of this embodiment are performed to obtain a laminate comprising a substrate, a first clad layer, and a base film in this order. When obtaining a laminate comprising a substrate, a first clad layer, and a base film in this order, step (C) may be further included. Thereafter, the base film is peeled from the laminate comprising a substrate, a first clad layer, and a base film in this order, and a film for forming a core layer is laminated to form the core layer. Next, a film for forming a second clad layer is laminated to form the second clad layer. Furthermore, steps such as forming a waveguide pattern in the core layer and forming a mirror on the optical waveguide may be appropriately included.

[0052] In the laminate of this embodiment, when the volume of the through hole formed in the substrate is taken as 100 volume %, from the viewpoint of further suppressing propagation loss of the optical waveguide, it is preferable that 70 volume % or more of the through hole is filled with the resin composition for forming the first clad layer. When the volume of the through hole is taken as 100 volume %, from the viewpoint of further suppressing propagation loss of the optical waveguide, the proportion of the resin composition for forming the first clad layer filled in the through hole is more preferably 75 volume % or more, even more preferably 80 volume % or more, even more preferably 85 volume % or more, even more preferably 90 volume % or more, even more preferably 95 volume % or more, even more preferably 98 volume % or more, even more preferably 99 volume % or more, and for example, 100 volume % or less. The resin composition for forming the first clad layer is a resin composition derived from the resin layer (a) of the resin film.

[0053] [Resin Film] The resin film having the resin layer (a) made of the resin composition for forming the first clad layer of this embodiment will be specifically described.

[0054] The thickness of the resin layer (a) is preferably 10 μm or more, more preferably 15 μm or more, and even more preferably 20 μm or more, from the viewpoint of further improving embeddability, and is preferably 300 μm or less, more preferably 250 μm or less, even more preferably 200 μm or less, even more preferably 100 μm or less, even more preferably 80 μm or less, even more preferably 60 μm or less, even more preferably 40 μm or less, and even more preferably 30 μm or less, from the viewpoint of further improving the light propagation efficiency of the optical waveguide.

[0055] The thickness of the resin layer (a) is preferably smaller than the thickness of the substrate, and is preferably 80% or less, more preferably 70% or less, even more preferably 65% ​​or less, even more preferably 60% or less, and even more preferably 55% or less, when the thickness of the substrate is 100%, and may be, for example, 10% or more, or 15% or more.

[0056] Here, the thickness of the resin layer (a) in this specification means the thickness of the resin layer (a) in step (A). That is, in the method for producing a laminate of this embodiment, the work is pressed in step (B), but the thickness of the resin layer (a) in this specification does not mean the thickness after pressing.

[0057] The resin contained in the resin layer (a) is not particularly limited as long as it is a resin that can be used to form a clad layer of an optical waveguide. Among them, the resin layer (a) preferably contains at least one selected from the group consisting of polyimide resins, compounds having a cyclic ether structure, and copolymers of styrene-based monomers and diene-based monomers.

[0058] The resin layer (a) more preferably contains a polyimide resin and a compound having a cyclic ether structure.

[0059] The polyimide resin in the resin layer (a) preferably contains an imide ring structure in the molecule. The polyimide resin in the resin layer (a) preferably contains a fluorinated polyimide. The fluorinated polyimide refers to a polyimide containing a fluorine atom.

[0060] The polyimide resin in the resin layer (a) may be a single polyimide resin, or may contain two or more polyimide resins.

[0061] The compound having a cyclic ether structure in the resin layer (a) preferably contains at least one or more selected from the group consisting of epoxy resins and oxetane compounds, and more preferably contains one or more epoxy resins.

[0062] The compound having a cyclic ether structure in the resin layer (a) preferably contains an alicyclic structure in its molecule. Here, the compound having a cyclic ether structure containing an alicyclic structure in its molecule means that it contains an alicyclic structure in addition to the cyclic ether structure. However, the alicyclic structure in this embodiment includes a fused ring structure in which a cyclic ether and an aliphatic ring are fused, and a spiro ring structure in which a cyclic ether and an aliphatic ring are bonded by a spiro bond atom. The number of ring members in the alicyclic structure is not particularly limited, but is preferably a 4- to 10-membered ring, more preferably a 4- to 8-membered ring, even more preferably a 5- or 6-membered ring, and even more preferably a 6-membered ring.

[0063] The compound having a cyclic ether structure in the resin layer (a) preferably contains two or more cyclic ether structures in the molecule, and more preferably contains two or three cyclic ether structures in the molecule.

[0064] The compound having a cyclic ether structure in the resin layer (a) may be a compound having one type of cyclic ether structure, or may contain two or more types of compounds having a cyclic ether structure.

[0065] The content of the polyimide resin contained in the resin layer (a) is preferably 20 parts by mass or more, more preferably 23 parts by mass or more, even more preferably 25 parts by mass or more, and even more preferably 28 parts by mass or more, from the viewpoint of further improving embeddability, when the total content of the resin components in the resin layer (a) is taken as 100 parts by mass. Also, from the viewpoint of further improving embeddability, the content is preferably 80 parts by mass or less, more preferably 75 parts by mass or less, even more preferably 70 parts by mass or less, and even more preferably 65 parts by mass or less.

[0066] The content of the compound having a cyclic ether structure contained in the resin layer (a) is preferably 20 parts by mass or more, more preferably 25 parts by mass or more, even more preferably 30 parts by mass or more, and even more preferably 35 parts by mass or more, when the total content of the resin components in the resin layer (a) is taken as 100 parts by mass, from the viewpoint of further improving embeddability, and is preferably 80 parts by mass or less, more preferably 75 parts by mass or less, from the viewpoint of further improving embeddability.

[0067] The total content of the polyimide resin and the compound having a cyclic ether structure contained in the resin layer (a) is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and still more preferably 97% by mass or more, when the total content of all components in the resin layer (a) is 100% by mass, and may be, for example, 99.5% by mass or less, or 99.0% by mass or less.

[0068] The resin layer (a) more preferably contains a copolymer of a styrene-based monomer and a diene-based monomer and a compound having a cyclic ether structure. Here, the copolymer of a styrene-based monomer and a diene-based monomer in this embodiment also includes a copolymer obtained by hydrogenating the copolymer of a styrene-based monomer and a diene-based monomer. The compound having a cyclic ether structure is as described above.

[0069] In the copolymer of a styrene-based monomer and a diene-based monomer, the styrene-based monomer refers to styrene and a monomer in which some of the hydrogen atoms of styrene have been substituted with alkyl groups, such as methyl, ethyl, and propyl groups.

[0070] In the copolymer of a styrene-based monomer and a diene-based monomer, examples of the diene-based monomer include 1,3-butadiene and isoprene.

[0071] Specific examples of copolymers of styrene-based monomers and diene-based monomers include styrene-butadiene rubber, styrene-butadiene-styrene (SBS) block copolymers, styrene-ethylene-butylene-styrene (SEBS) block copolymers, styrene-ethylene-propylene (SEP) block copolymers, and styrene-ethylene-ethylene-propylene-styrene (SEEPS) block copolymers. Commercially available copolymers of styrene-based monomers and diene-based monomers include SEPTON (registered trademark, manufactured by Kuraray Co., Ltd.) and Tuftec (registered trademark, manufactured by Asahi Kasei Corporation).

[0072] The copolymer of a styrene-based monomer and a diene-based monomer in the resin layer (a) may be a single copolymer, or may contain two or more types of copolymers.

[0073] The total content of the copolymer of a styrene-based monomer and a diene-based monomer and the compound having a cyclic ether structure contained in the resin layer (a) is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, when the total content of all components in the resin layer (a) is 100% by mass, and may be, for example, 99% by mass or less, or 98% by mass or less.

[0074] The resin layer (a) may contain, in addition to the resin component, components such as a curing agent and a surfactant, as appropriate.

[0075] When the total content of all components in the resin layer (a) is taken as 100% by mass, the content of the (meth)acrylic resin contained in the resin layer (a) is preferably less than 50% by mass, more preferably less than 30% by mass, even more preferably less than 10% by mass, even more preferably less than 5% by mass, even more preferably less than 1% by mass, even more preferably less than 0.1% by mass, and even more preferably 0% by mass, from the viewpoint of further improving the heat resistance of the resin layer (a). Here, the term "(meth)acrylic resin" is used as a concept including both methacrylic resin and acrylic resin.

[0076] When the complex viscosity of the resin layer (a) is measured by a melt viscoelasticity test under the conditions of a measurement frequency of 10 rad / sec, a temperature range of 23°C to 200°C, and a temperature increase rate of 3°C / min, the complex viscosity η* at 100°C is preferably 1.0 x 10 3 Pa s or more, more preferably 2.0 × 10 3 Pa s or more, more preferably 3.0 × 10 3 Pa s or more, more preferably 4.0 × 10 3 Pa s or more, more preferably 5.0 × 10 3 From the viewpoint of further improving embeddability, the viscosity is preferably 1.0×10 7 Pa s or less, more preferably 1.0 × 10 6 Pa s or less, more preferably 5.0 × 10 5 Pa s or less, more preferably 1.0 × 10 5 Pa s or less, more preferably 9.5 × 10 4 Pa s or less, more preferably 9.3 × 10 4 Pa s or less, more preferably 9.0 × 10 4 Pa s or less, more preferably 8.8 × 10 4 It is less than Pa·s.

[0077] When the complex viscosity of the resin layer (a) is measured by a melt viscoelasticity test under the conditions of a measurement frequency of 10 rad / sec, a temperature range of 23°C to 200°C, and a heating rate of 3°C / min, the temperature at which the complex viscosity η* is minimum is preferably 70°C or higher, more preferably 80°C or higher, and even more preferably 90°C or higher, and from the viewpoint of further improving embeddability, is preferably 180°C or lower, more preferably 170°C or lower, even more preferably 160°C or lower, and even more preferably 140°C or lower.

[0078] The complex viscosity η* of the resin layer (a) can be adjusted to a desired range by, for example, adjusting the type of resin constituting the resin layer (a), the weight-average molecular weight (Mw) and glass transition temperature, the content ratio of the components of the resin layer (a), etc. More specifically, the complex viscosity η* can be adjusted to a desired range by, for example, including a polyimide resin and a compound having a cyclic ether structure in the resin layer (a).

[0079] The resin film of this embodiment preferably further includes a substrate film, and more preferably includes a resin layer (a) on the substrate film. The substrate film may be, for example, a resin film. The resin constituting the substrate film is not particularly limited, but preferably includes at least one or more resins selected from the group consisting of polyimide and polyethylene terephthalate, and more preferably includes polyethylene terephthalate.

[0080] From the viewpoint of further improving the handleability of the film, the thickness of the base film of the present embodiment is preferably 10 μm or more, more preferably 15 μm or more, even more preferably 20 μm or more, preferably 30 μm or more, and is preferably 100 μm or less, more preferably 80 μm or less, even more preferably 60 μm or less, even more preferably 40 μm or less.

[0081] The substrate film of the present embodiment may be subjected to a surface treatment such as an antistatic treatment or a release treatment.

[0082] The resin film of this embodiment can be obtained, for example, by applying a resin composition for forming the first clad layer onto a substrate film and drying it to form a resin layer (a). When applying the resin composition for forming the first clad layer onto the substrate film, the resin composition is preferably a varnish-like resin composition containing an organic solvent. The organic solvent in the resin composition is removed in the drying process. Examples of application methods include direct application using various coater devices such as a pin coater, die coater, comma coater, and curtain coater, and printing methods such as screen printing.

[0083] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various other configurations may be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of achieving the object of the present invention are included in the present invention.

[0084] The present embodiment will be described in detail below based on examples and comparative examples, but the present embodiment is not limited to the descriptions of these examples.

[0085] [Preparation of Resin Film] Preparation of a resin film having a resin layer (a) made of a resin composition for forming a first clad layer will be described. First, each raw material constituting the resin composition for forming the first clad layer will be described.

[0086] (Synthesis of Polyimide Resin (A-1)) A 3 L separable glass flask equipped with a stirrer and a stirring blade was charged with 67.3 g (0.210 mol) of 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 97.7 g (0.220 mol) of 4,4'-(hexafluoroisopropylidene)diphthalic dianhydride, and 495 g of dimethylacetamide, and the mixture was stirred to dissolve. Further, stirring was continued at room temperature for 12 hours under a nitrogen stream to carry out a polymerization reaction, yielding a polyamic acid solution.

[0087] To the resulting polyamic acid solution, 16 g of pyridine was added, and then 82 g of acetic anhydride was added dropwise at room temperature. Thereafter, the liquid temperature was maintained at 20 to 100°C and stirring was continued for 24 hours to carry out the imidization reaction, thereby obtaining a polyimide solution.

[0088] The obtained polyimide solution was poured into 1,000 g of methanol in a 5 L container while stirring to precipitate a polyimide resin. Thereafter, the solid polyimide resin was filtered using a suction filtration device and further washed with 1,000 g of methanol. Then, the solid polyimide resin was dried at 100°C for 24 hours using a vacuum dryer and further dried at 200°C for 3 hours to obtain a powdery polyimide resin (A-1). The weight average molecular weight (Mw) of the polyimide resin (A-1) measured by GPC was 51,000. 1H-NMR was measured, and the imidization rate was calculated from the quantitative value of the amide peak relative to the peak of the aromatic ring of the polyimide, and the imidization rate was found to be 99% or more. Polyimide resin (A-1) was dissolved in propylene glycol monomethyl ether acetate to a solids concentration of 25%, and then coated using an applicator to a film thickness of 30 μm. The film was then dried in an oven at 100°C for 10 minutes to obtain a polyimide coating. The refractive index of the resulting coating was measured using an Abbe refractometer (manufactured by Atago Co., Ltd., product name: NAR-1T SOLID) under conditions of 23°C and 589 nm, and the refractive index of the polyimide was found to be 1.54.

[0089] Details of the raw materials in Table 1 are as follows:

[0090] <Polymer (A)> (A-1) The polyimide resin synthesized above (Mw=51,000, imidization rate of 99% or more, refractive index n=1.54) (A-2) Rubber-based elastomer (manufactured by Kuraray Co., Ltd., product name: Septon Q1250, copolymer of styrene-based monomer and diene-based monomer, Mw=100,000, refractive index n=1.50)

[0091]

[0092] <Compound (B) Having a Cyclic Ether Structure> (B-1) Celloxide 2021P (manufactured by Daicel Corporation, epoxy resin having an alicyclic structure, liquid at 23°C, refractive index 1.51)

[0093] <Curing Agent (C)> (C-1) San-Aid SI-110 (manufactured by Sanshin Chemical Industry Co., Ltd., thermal cationic polymerization initiator) (C-2) San-Aid SI-150 (manufactured by Sanshin Chemical Industry Co., Ltd., thermal cationic polymerization initiator) (C-3) San-Aid SI-B3 (manufactured by Sanshin Chemical Industry Co., Ltd., thermal cationic polymerization initiator)

[0094] <Surfactant (D)> (D-1) BYK-333 (manufactured by BYK Japan KK, silicone surfactant) (D-2) BYK-361 (manufactured by BYK Japan KK, acrylic polymer surfactant)

[0095] <Organic Solvent (E)> (E-1) Propylene glycol monomethyl ether acetate (E-2) Propylene glycol monomethyl ether (E-3) Toluene

[0096] <Preparation of Resin Composition> The raw materials formulated according to Table 1 were stirred at room temperature until the raw materials were completely dissolved to obtain a solution. The solution was then filtered through a PTFE filter with a pore size of 0.2 μm to obtain varnish-like resin compositions of clad A and clad B, respectively.

[0097] <Preparation of Resin Film> The varnish-like resin compositions of Clad A and Clad B obtained by preparing the resin composition described above were applied to a 38 μm thick antistatically treated polyethylene terephthalate substrate (manufactured by Nippa Corporation, product name: PET38x1-TR1-ASQ, hereinafter referred to as PET substrate) using an applicator so that the dried thickness would be 25 μm. The varnish was then dried at 100° C. for 10 minutes, and finally an OPP cover film (manufactured by Oji F-Tex Co., Ltd., product name: E201F-50 μm) was attached to the surface of the resin layer formed from the resin composition to obtain a resin film. Note that for the resin film having a thickness of 25 μm for resin layer (a) in Table 2, the resin film obtained by the above method was used as is. Resin films in Table 2 having a resin layer (a) with a thickness of more than 25 μm were prepared by laminating resin films having a resin layer (a) with a thickness of 25 μm in a laminating machine under the conditions of a temperature of 30°C, a pressure of 1.0 MPa, and a time of 120 seconds until the specified resin layer (a) thickness was achieved.

[0098] [Examples 1 to 10 and Comparative Examples 1 to 3] <Workpiece Preparation Step (A)> The OPP cover film was peeled off from the resin film, and a workpiece was prepared in which a resin film was placed on a double-sided copper-clad laminate (CCL) having a through hole so that the resin layer (a) of the resin film was in contact with the double-sided copper-clad laminate. The layer structure of the workpiece was "double-sided copper-clad laminate / resin layer (a) / PET substrate." The type of clad material of the resin film and the thickness of the resin layer (a) are shown in Table 2. The thickness T of the double-sided copper-clad laminate, the hole diameter R of the through hole, and T / R are also shown in Table 2.

[0099] <Laminating step (B)> The resin layer (a) was laminated onto the double-sided copper-clad laminate by pressing the workpiece under the conditions described in step (B) in Table 2. The "rubber" listed for the laminating device in Table 2 means that the workpiece was pressed using the first stage of a rubber press laminator (manufactured by Nikko Materials Co., Ltd., product name: CVP-600). The "diaphragm" listed for the laminating device in Table 2 means that the workpiece was pressed using the first stage of a diaphragm laminator (manufactured by Nikko Materials Co., Ltd., product name: CVP-300).

[0100] <Pressing Step (C)> After step (B), the workpiece was further pressed under normal pressure conditions based on the conditions described in step (C) in Table 2, to obtain laminates of Examples 1 to 10 and Comparative Examples 1 to 3. In the Examples and Comparative Examples in which the laminating device in step (B) described in Table 2 was "Rubber," the workpiece was pressed using the 2nd stage of a rubber press laminator (manufactured by Nikko Materials Co., Ltd., product name: CVP-600). In the Examples in which the laminating device in step (B) described in Table 2 was "Diaphragm," the workpiece was pressed using the 2nd stage of a diaphragm laminator (manufactured by Nikko Materials Co., Ltd., product name: CVP-300).

[0101] [Measurement and Evaluation] <Measurement of complex viscosity η* of resin layer (a)> A resin film having a resin layer (a) thickness of 25 μm was laminated with a laminator under conditions of temperature: 30 ° C, pressure: 1.0 MPa, and time: 120 seconds so that the resin layer (a) had a thickness of 100 μm, to obtain a sample for complex viscosity measurement. More specifically, two films were laminated to produce two films with a resin layer thickness of 50 μm, and then two films with a resin layer thickness of 50 μm were laminated to obtain a sample with a resin layer thickness of 100 μm. When obtaining the sample for complex viscosity measurement, the PET substrate and OPP cover film were appropriately removed. The melt viscoelasticity of the sample for complex viscosity measurement was measured using a viscoelasticity measuring device (manufactured by Anton Paar Japan, product name: MCH302) at a frequency of 10 rad / sec, while changing the temperature from 23°C to 200°C at a heating rate of 3°C / min. From the results obtained, the complex viscosity η* [Pa s] at 100°C at 10 rad / sec and the temperature [°C] at which the complex viscosity η* at a frequency of 10 rad / sec is minimum were calculated. The measurement results of the complex viscosity η* are shown in Table 1.

[0102] <Evaluation of Fillability> For the laminates of Examples 1 to 10 and Comparative Examples 1 to 3, the through holes in the substrate were observed under a microscope and evaluated according to the following criteria: A (very good): Filled with no voids. B (good): Filled with some voids. C (poor): Not filled. The results of the fillability evaluation are shown in Table 2.

[0103]

[0104]

[0105] It can be seen from Table 2 that all of the laminates obtained by the manufacturing methods of the examples had good embeddability evaluations. That is, according to the manufacturing method of the laminate of this embodiment, a laminate can be obtained that can produce an optoelectronic composite substrate with improved embeddability.

[0106] This application claims priority based on Japanese Patent Application No. 2023-057399, filed March 31, 2023, the disclosure of which is incorporated herein in its entirety by reference.

[0107] 20 First cladding layer 30 Core layer 40 Second cladding layer 50 Mirror on the light-emitting element side 60 Mirror on the light-receiving element side 100 Optical waveguide 110 Substrate 120 Light-emitting element 130 Light-receiving element 140a, 140b Through-hole 200 Optoelectronic composite substrate 300 Resin film 310 Resin layer (a) 320 Base film 400 Work

Claims

1. A method for manufacturing a laminate comprising a substrate having a through hole and a first clad layer of an optical waveguide, comprising at least the steps of: (A) preparing a workpiece on which a resin film having a resin layer (a) made of a resin composition for forming the first clad layer is placed on the substrate; and (B) laminating the first clad layer onto the substrate by heating and pressing the workpiece under reduced pressure using a vacuum laminating device.

2. The method for producing a laminate according to claim 1, wherein, when the thickness of the substrate is T [μm] and the diameter of the through hole is R [μm], T / R is 0.10 or more.

3. The method for producing a laminate according to claim 1 or 2, wherein the through holes have a diameter of 10 μm or more and 1000 μm or less.

4. The method for producing a laminate according to any one of claims 1 to 3, wherein the thickness of the substrate is 10 μm or more and 1000 μm or less.

5. The method for producing a laminate according to any one of claims 1 to 4, wherein the thickness of the resin layer (a) is 10 μm or more and 300 μm or less.

6. The method for producing a laminate according to any one of claims 1 to 5, wherein the thickness of the resin layer (a) is smaller than the thickness of the substrate.

7. The resin layer (a) has a complex viscosity η* of 1.0×10 at 100° C. when the complex viscosity is measured by a melt viscoelasticity test under the conditions of a measurement frequency of 10 rad / sec, a temperature range of 23° C. to 200° C., and a temperature rise rate of 3° C. / min. 3 Pa・s or more 1.0×10 7 The method for producing a laminate according to any one of claims 1 to 6, wherein the viscosity is Pa·s or less.

8. A method for producing a laminate according to any one of claims 1 to 7, wherein the resin layer (a) contains at least one selected from the group consisting of polyimide resins, compounds having a cyclic ether structure, and copolymers of styrene-based monomers and diene-based monomers.

9. The method for producing a laminate according to any one of claims 1 to 8, wherein in step (B), the work is heated to 80°C or higher and 190°C or lower and pressed.

10. A method for producing a laminate according to any one of claims 1 to 9, wherein in step (B), the workpiece is sandwiched between two press plates and heated and pressed.

11. The method for producing a laminate according to claim 10, wherein in step (B), at least one of the two press plates comprises rubber.

12. The method for producing a laminate according to any one of claims 1 to 11, wherein in the step (B), the degree of vacuum is 500 Pa or less.

13. A method for producing a laminate according to any one of claims 1 to 12, wherein in step (B), the pressure applied when pressing the workpiece is 0.3 MPa or more and 10.0 MPa or less.

14. A method for producing a laminate according to any one of claims 1 to 13, further comprising, after step (B), a step (C) of sandwiching the workpiece between two press plates and heating and pressing the workpiece.

15. A method for manufacturing a laminate described in any one of claims 1 to 14, wherein, when the volume of the through hole of the laminate is 100 volume %, 70 volume % or more of the through hole is filled with a resin composition for forming the first clad layer.

16. A method for producing a laminate according to any one of claims 1 to 15, wherein the laminate is an optical / electrical composite substrate further comprising a core layer and a second clad layer, in that order, on the first clad layer.

Citation Information

Patent Citations

  • Optical waveguide structure, its manufacturing method, and optical waveguide device

    JP2005331779A

  • Substrate with lens and production method therefor, and optical waveguide with lens

    JP2014041181A

  • Optical waveguide and method for manufacturing the same

    JP2014066751A

  • Adhesive sheet, optical waveguide with adhesive sheet, photo-electric hybrid board, method for manufacturing photo-electric hybrid board, optical module, and electronic equipment

    JP2015114390A

  • Optical waveguide with lens, photo-electric hybrid substrate, optical module and electronic apparatus

    JP2017125956A