Rubber composition for undertreads

The rubber composition for undertreads, combining isoprene and unmodified butadiene rubber with specific silica and carbon black, addresses the balance of handling stability, high-speed durability, and low heat generation, achieving improved tire performance.

WO2024204358A1PCT designated stage expired Publication Date: 2024-10-03THE YOKOHAMA RUBBER CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012266
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current rubber compositions for undertreads in tires face challenges in balancing handling stability, high-speed durability, and low heat generation, as methods to reduce heat generation, such as increasing vulcanizing agents or decreasing carbon black, compromise elongation at break and durability.

Method used

A rubber composition comprising 60-90% isoprene rubber, 10-40% unmodified butadiene rubber, large particle size silica, and specific carbon black, along with a silane coupling agent, optimized to improve handling stability, high-speed durability, and low heat generation by controlling molecular weight distribution and filler ratios.

Benefits of technology

The composition effectively enhances handling stability, high-speed durability, and maintains low heat generation, ensuring well-balanced performance in tire undertreads.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012266_03102024_PF_FP_ABST
    Figure JP2024012266_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a rubber composition for undertreads, which provides improved maneuvering stability and high-speed durability while ensuring good low-heat-generating properties and allows for a high level of balance among these properties. In the present invention, 3-60 parts by mass of silica having a CTAB adsorption specific surface area of 60-100 m2 / g is added to 100 parts by mass of a rubber component containing 60-90 mass% of an isoprene rubber and 10-40 mass% of an unmodified butadiene rubber. As the unmodified butadiene rubber, one having a molecular weight distribution (Mw / Mn), as determined from the weight average molecular weight (Mw) and the number average molecular weight (Mn), of at most 2.8 is used.<sp / >
Need to check novelty before this filing date? Find Prior Art

Description

Rubber composition for undertread

[0001] The present invention relates to a rubber composition for undertreads intended primarily for use in the undertread layer of tires.

[0002] In pneumatic tires, there is a demand for improving fuel economy during driving in order to reduce environmental impact. To this end, efforts have been made to suppress heat generation in rubber compositions constituting various parts of pneumatic tires. In recent years, in order to further improve fuel economy, for example, studies have been made on suppressing heat generation in rubber compositions constituting the undertread rubber layer of pneumatic tires (rubber compositions for undertread).

[0003] As an index of heat buildup of a rubber composition, tan δ at 60°C (hereinafter referred to as "tan δ (60°C)") measured by dynamic viscoelasticity measurement is generally used, and the smaller the tan δ (60°C) of the rubber composition, the smaller the heat buildup. Methods for reducing the tan δ (60°C) of a rubber composition include, for example, increasing the compounding amount of a vulcanizing agent or reducing the compounding amount of a filler such as carbon black (see, for example, Patent Document 1). However, these methods do not sufficiently ensure the breaking elongation required for a rubber composition for an undertread, and there is a risk that sufficient steering stability and high-speed durability of the tire may not necessarily be obtained. Therefore, there is a demand for further measures for improving steering stability and high-speed durability while ensuring good low heat buildup (tan δ (60°C)) in a rubber composition for an undertread.

[0004] Japanese Patent Application Publication No. 2013-177113

[0005] An object of the present invention is to provide a rubber composition for an undertread which improves steering stability and high-speed durability while ensuring good low heat buildup, thereby achieving a high degree of compatibility between these performances in a well-balanced manner.

[0006] The rubber composition for undertread of the present invention, which achieves the above object, comprises a rubber component containing 60 to 90% by mass of isoprene-based rubber and 10 to 40% by mass of unmodified butadiene rubber, and a CTAB adsorption specific surface area of ​​60 m2 / g to 100m 2 / g, and the molecular weight distribution (Mw / Mn) calculated from the weight average molecular weight (Mw) and number average molecular weight (Mn) of the unmodified butadiene rubber is 2.8 or less.

[0007] The rubber composition for undertread of the present invention, which is made up of the above-mentioned blending, can improve steering stability and high-speed durability while ensuring good low heat buildup. Specifically, by using an isoprene-based rubber and an unmodified butadiene rubber in the above-mentioned blending ratio as the rubber component, it is possible to improve low heat buildup and high-speed durability in a well-balanced manner. In addition, by adding large particle size silica (having a CTAB adsorption specific surface area of ​​60 m) to this rubber component, 2 / g to 100m 2 / g) is blended in an appropriate amount, thereby improving low heat buildup. Furthermore, the unmodified butadiene rubber used has a molecular weight distribution (Mw / Mn) of 2.8 or less, which effectively improves the handling stability and high-speed durability of the resulting tire while maintaining good low heat buildup. These factors work together to ensure good low heat buildup, while improving handling stability and high-speed durability, achieving a good balance between these performance characteristics.

[0008] In the present invention, the CTAB adsorption specific surface area is 40 m per 100 parts by mass of the rubber component. 2 / g~120m 2 It is preferable that 20 to 70 parts by mass of carbon black having a specific particle size be blended as a filler in addition to the large particle size silica described above. By blending an appropriate amount of carbon black having a specific particle size as a filler, it is possible to improve processability (rubber cohesion, adhesion to other components, etc.).

[0009] In the present invention, the unmodified butadiene rubber preferably has a cis-1,4 bond content of 95% or more. Furthermore, the unmodified butadiene rubber preferably has a viscosity Tcp (unit: cps) of a 5% by mass toluene solution at 25°C and a Mooney viscosity ML at 100°C. 1+4 Ratio of Tcp / ML 1+4It is preferable that the relationship between the ratio of the modified butadiene rubber and the high-speed durability be satisfied, and that the ratio of the modified butadiene rubber and the high-speed durability be satisfied is 2.0 to 7.0. In addition, it is preferable that the unmodified butadiene rubber be synthesized using a neodymium-based catalyst. By using an unmodified butadiene rubber that satisfies these specific conditions, the effects of improving the low heat buildup and high-speed durability described above can be enhanced, and this is advantageous for improving the handling stability and high-speed durability while maintaining good low heat buildup.

[0010] In the present invention, a silane coupling agent can be blended, and in this case, the ratio of the blended amount of the silane coupling agent to the blended amount of silica is preferably 3.0% by mass to 10.0% by mass, which can improve the dispersion of the silica and is advantageous for improving low heat buildup and high-speed durability.

[0011] The rubber composition for an undertread of the present invention can be suitably used in the undertread layer of a tire. Specifically, a tire using the rubber composition for an undertread of the present invention has a tread portion extending in the tire circumferential direction to form an annular shape, and a pair of sidewall portions disposed on both sides of the tread portion, and the tread portion is preferably constructed by laminating a cap tread layer constituting the tire tread surface and an undertread layer disposed on the inner circumferential side of the cap tread layer. In such a tire, it is preferable that the undertread layer is constructed from the rubber composition for an undertread of the present invention. In this way, a tire having an undertread layer made from the rubber composition for an undertread of the present invention can improve steering stability and high-speed durability while ensuring good low heat buildup due to the excellent physical properties of the rubber composition for an undertread of the present invention.

[0012] At this time, the tensile stress M100 of the undertread rubber constituting the undertread layer at 23°C when elongated to 100% UT [unit: MPa] and the tensile stress M100 of the side rubber constituting the sidewall portion at 23°C when elongated to 100% SW Ratio M100 [unit: MPa] UT / M100 SWIt is preferable that the tensile stress (M100) is 1.5 to 4.0. By optimizing the relationship between the tensile stress (M100) of the undertread layer using the rubber composition for an undertread of the present invention and the adjacent sidewall portion (side rubber) in this way, it is advantageous to improve low heat buildup and high-speed durability.

[0013] In the present invention, the "CTAB adsorption specific surface area" is measured in accordance with ISO 5794. The "weight average molecular weight Mw" and the "number average molecular weight Mn" are measured by gel permeation chromatography (GPC) in terms of standard polystyrene. The "cis-1,4 bond content" is the proportion of cis-1,4 bonds among the cis-1,4-bonds, trans-1,4-bonds, and 1,2-vinyl bonds, which are the bonding modes of butadiene, and is measured by infrared spectroscopy (Hampton method). The "Mooney viscosity at 100°C ML 1+4 " is measured in accordance with JIS K6300-1:2001 using a Mooney viscometer with an L-type rotor, with a preheating time of 1 minute, a rotor rotation time of 4 minutes, and at 100°C. "Viscosity of a 5 mass% toluene solution at 25°C, Tcp" is the viscosity of a toluene solution containing 5% by weight of the target butadiene rubber, and is measured at 25°C using a Cannon-Fenske viscometer. "Tensile stress at 100% elongation at 23°C" is a value measured in accordance with JIS K6251 using a No. 3 dumbbell test piece at a tensile speed of 500 mm / min and a temperature of 23°C.

[0014] FIG. 1 is a meridian cross-sectional view showing an example of a pneumatic tire using the rubber composition for an undertread of the present invention.

[0015] The configuration of the present invention will be described in detail below with reference to the accompanying drawings.

[0016] As shown in Figure 1, a pneumatic tire in which the rubber composition for an undertread of the present invention is used includes a tread portion 1, a pair of sidewall portions 2 arranged on both sides of the tread portion 1, and a pair of bead portions 3 arranged radially inward of the sidewall portions 2. In Figure 1, the symbol CL indicates the tire equator. Although not depicted in Figure 1 because it is a meridian cross-section, the tread portion 1, sidewall portions 2, and bead portions 3 each extend in the tire circumferential direction and form an annular shape, thereby constituting the basic toroidal structure of a pneumatic tire. The following explanation using Figure 1 will be basically based on the meridian cross-section shape shown, but each tire constituent member also extends in the tire circumferential direction and forms an annular shape.

[0017] A carcass layer 4 is installed between a pair of left and right bead portions 3. This carcass layer 4 includes multiple reinforcing cords extending in the tire radial direction and folded back from the inner side to the outer side in the tire width direction around bead cores 5 arranged in each bead portion 3. A bead filler 6 is arranged on the outer periphery of each bead core 5, and this bead filler 6 is wrapped by the main portion and folded back portion of the carcass layer 4. Meanwhile, multiple belt layers 7 (two layers in FIG. 1 ) are embedded on the outer periphery of the carcass layer 4 in the tread portion 1. Each belt layer 7 includes multiple reinforcing cords inclined with respect to the tire circumferential direction, and the reinforcing cords are arranged so as to cross each other between the layers. In these belt layers 7, the inclination angle of the reinforcing cords with respect to the tire circumferential direction is set, for example, in the range of 10° to 40°. Furthermore, a belt reinforcing layer 8 (two layers: a full cover 8a covering the entire width of the belt layer 7 and an edge cover 8b locally covering the ends of the belt layer 7) is provided on the outer periphery of the belt layer 7. The belt reinforcing layer 8 includes organic fiber cords oriented in the tire circumferential direction. In the belt reinforcing layer 8, the organic fiber cords are angled at an angle of, for example, 0° to 5° with respect to the tire circumferential direction.

[0018] A tread rubber layer 10 is disposed on the outer peripheral side of the carcass layer 4 in the tread portion 1, a side rubber layer 20 is disposed on the outer peripheral side (outside in the tire width direction) of the carcass layer 4 in the sidewall portion 2, and a rim cushion rubber layer 30 is disposed on the outer peripheral side (outside in the tire width direction) of the carcass layer 4 in the bead portion 3. The tread rubber layer 11 has a structure in which two types of rubber layers with different physical properties (a cap tread 11 that forms the tread surface of the tread portion 1 and an undertread 12 disposed on its inner peripheral side) are laminated in the tire radial direction.

[0019] The tire in which the rubber composition for an undertread of the present invention is used is preferably a pneumatic tire (a tire filled with air, an inert gas such as nitrogen, or other gases) as described above, but may also be a non-pneumatic tire. In the case of a non-pneumatic tire, the rubber composition for an undertread of the present invention can be used in a rubber layer (a portion corresponding to the undertread layer 12 in a pneumatic tire) arranged on the inner circumferential side of the portion that contacts the road surface (a portion corresponding to the cap tread layer 11 in a pneumatic tire). As long as the tread portion 1 (tread rubber layer 10) of the tire to which the present invention is applied is composed of the cap tread 11 and the undertread 12, the basic structure of the other portions is not limited to the above-mentioned structure.

[0020] In the rubber composition for undertread of the present invention, the rubber component is a diene rubber, and necessarily contains an isoprene rubber and an unmodified butadiene rubber. In this way, using an isoprene rubber and an unmodified butadiene rubber is advantageous in improving low heat buildup while maintaining good elongation at break.

[0021] Examples of isoprene-based rubbers include various natural rubbers, epoxidized natural rubbers, and various synthetic polyisoprene rubbers. Among these isoprene-based rubbers, natural rubber is particularly suitable. The content of the isoprene-based rubber is 60% to 90% by mass, preferably 65% ​​to 90% by mass, and more preferably 70% to 90% by mass, based on 100% by mass of the rubber component. By including such an amount of isoprene-based rubber (particularly natural rubber), it is possible to achieve a balanced improvement in elongation at break and low heat buildup. If the amount of isoprene-based rubber is less than 60% by mass, the elongation at break decreases. If the amount of isoprene-based rubber is more than 90% by mass, the low heat buildup decreases.

[0022] The unmodified butadiene rubber used has a molecular weight distribution (Mw / Mn) calculated from the weight average molecular weight (Mw) and number average molecular weight (Mn) of 2.8 or less, preferably 2.5 or less. By using an unmodified butadiene rubber with an appropriate molecular weight distribution, the rubber physical properties are improved, and the handling stability and high-speed durability of the resulting tire can be effectively improved while maintaining low heat buildup. If the molecular weight distribution (Mw / Mn) of the unmodified butadiene rubber exceeds 2.8, the hysteresis loss increases, the heat buildup of the rubber increases, and the compression set resistance decreases.

[0023] The content of the unmodified butadiene rubber is 10% by mass to 40% by mass, preferably 15% by mass to 35% by mass, and more preferably 20% by mass to 35% by mass, based on 100% by mass of the rubber component. Such an appropriate content of unmodified butadiene rubber is advantageous for achieving a balanced improvement in elongation at break and low heat buildup. If the blending amount of unmodified butadiene rubber is less than 10% by mass, low heat buildup deteriorates. If the blending amount of unmodified butadiene rubber exceeds 40% by mass, elongation at break decreases.

[0024] The cis-1,4 bond content of unmodified butadiene rubber is preferably 95% or more, more preferably 96% to 99%. A high cis-1,4 bond content is advantageous for improving strength at break and elongation at break. If the cis-1,4 bond content is less than 95%, strength at break and elongation at break decrease. The cis-1,4 bond content of butadiene rubber can be increased or decreased by a conventional method such as using a catalyst.

[0025] The viscosity of a 5% by mass toluene solution of unmodified butadiene rubber at 25°C, Tcp (unit: cps), and the Mooney viscosity at 100°C, ML 1+4 Ratio of Tcp / ML 1+4 The ratio Tcp / ML preferably satisfies the relationship of 2.0 to 7.0, and more preferably 2.5 to 6.8. 1+4 By setting the ratio Tcp / ML within a specific range, it is advantageous to achieve low heat buildup, breaking strength, and breaking elongation all at once. 1+4 If the ratio Tcp / ML is less than 2.0, the low heat buildup property is deteriorated. 1+4 If it exceeds 7.0, the processability deteriorates.

[0026] The above-mentioned ratio Tcp / ML 1+4 In setting the Mooney viscosity ML at 100°C, the value of the viscosity Tcp of a 5% by mass toluene solution at 25°C is not particularly limited, but it can be set preferably to 50 cps to 200 cps, more preferably to 80 cps to 180 cps. 1+4 The value of the saturation voltage itself is not particularly limited, but it can be set preferably to 45 to 52, more preferably to 45 to 50.

[0027] The unmodified butadiene rubber is preferably butadiene rubber synthesized using a neodymium catalyst (hereinafter, sometimes referred to as Nd-BR). Although the desired effects can be obtained by using butadiene rubber polymerized with other catalysts (e.g., nickel or cobalt), Nd-BR is preferably used from the viewpoint of achieving both low heat buildup, high strength at break, and high elongation at break.

[0028] Note that butadiene rubber polymerized using a neodymium-based catalyst (Nd-BR) is a known material, and is butadiene rubber polymerized using a neodymium-based catalyst such as simple neodymium, compounds of neodymium with other metals, or organic neodymium compounds. Butadiene rubber synthesized using these neodymium-based catalysts has the characteristics of a high molecular weight and a narrow molecular weight distribution. Commercially available Nd-BR can be used.

[0029] The rubber component constituting the rubber composition for undertread of the present invention includes at least two types of rubber: the isoprene-based rubber (particularly natural rubber) and unmodified butadiene rubber described above, but may optionally contain other diene-based rubbers. As the other diene-based rubber, rubbers that can generally be used in rubber compositions for tires can be used. For example, unmodified styrene-butadiene rubber can be exemplified. Furthermore, when natural rubber is used as the isoprene-based rubber, isoprene rubber can also be used in combination as the other diene-based rubber. These other diene-based rubbers can be used alone or in any blend.

[0030] In the present invention, silica is always blended as a filler into the rubber component. The silica used in the present invention may be, for example, a silica typically used in rubber compositions for tires, such as wet-process silica, dry-process silica, or surface-treated silica. However, the CTAB adsorption specific surface area of ​​the silica must be 60 m. 2 / g to 100m 2 / g, preferably 70m 2 / g~90m 2 / g, more preferably 75m 2 / g~85m 2 / g. By using silica with such a large particle size, it is possible to improve low heat buildup and wear resistance. 2 When the CTAB adsorption specific surface area of ​​the silica is less than 100 m / g, the low heat buildup property is deteriorated. 2 If the silica satisfies the above conditions, it may be selected from commercially available silicas, or silica obtained by a conventional manufacturing method may be used.

[0031] The amount of silica compounded is 3 to 60 parts by mass, preferably 5 to 50 parts by mass, and more preferably 10 to 50 parts by mass, per 100 parts by mass of the rubber component. By compounding an appropriate amount of silica in this way, it is possible to improve the low heat buildup, steering stability, and high-speed durability of a tire in a well-balanced manner. If the amount of silica compounded is less than 3 parts by mass, the elongation at break decreases. If the amount of silica compounded exceeds 60 parts by mass, the low heat buildup deteriorates.

[0032] In the present invention, in addition to the silica described above, carbon black can also be compounded as a filler. The carbon black used in the present invention is preferably a carbon black having a CTAB adsorption specific surface area of ​​40 m among the carbon blacks normally used in rubber compositions for tires. 2 / g~120m 2 / g, more preferably 70m 2 / g to 100m 2 / g. The use of such carbon black is advantageous in improving the balance of low heat buildup, steering stability, and high-speed durability when made into a tire. 2 When the CTAB adsorption specific surface area of ​​the carbon black is less than 120 m / g, the abrasion resistance is reduced. 2 If it exceeds 1 / g, the low heat buildup property deteriorates.

[0033] When carbon black is used in addition to silica as described above, the total amount of silica and carbon black is preferably 40 to 95 parts by mass, more preferably 45 to 90 parts by mass, per 100 parts by mass of the rubber component. Blending appropriate amounts of silica and carbon black in this way is advantageous for achieving a balanced improvement in the low heat buildup, handling stability, and high-speed durability of the resulting tire. If the total amount of silica and carbon black is less than 40 parts by mass, the breaking strength decreases and high-speed durability deteriorates. If the total amount of silica and carbon black exceeds 95 parts by mass, fuel economy deteriorates and elongation at break decreases.

[0034] Furthermore, when silica and carbon black are used in combination, the ratio Ms / Mc of the amount of silica blended to the amount of carbon black blended, Mc, is preferably 0.05 to 0.7, more preferably 0.1 to 0.6. Blending silica and carbon black in this way in an appropriate balance, and particularly keeping the amount of silica in the filler low, can suppress the deterioration of tan δ (60°C) caused by blending large-particle silica, and can improve elongation at break and low heat buildup in a balanced manner. If the ratio Ms / Mc of the amount of silica blended to the amount of carbon black blended exceeds 0.7, processability (e.g., rubber cohesion, adhesion to other components) deteriorates.

[0035] The rubber composition of the present invention may contain fillers other than silica and carbon black, such as clay, talc, calcium carbonate, mica, aluminum hydroxide, and other materials commonly used in rubber compositions for tires.

[0036] In the rubber composition for undertread of the present invention, a silane coupling agent may be compounded when compounding the silica. Compounding a silane coupling agent can improve the dispersibility of silica in the rubber component (diene rubber). Examples of silane coupling agents include bis-(3-triethoxysilylpropyl)tetrasulfide, bis(3-triethoxysilylpropyl)disulfide, 3-trimethoxysilylpropylbenzothiazoletetrasulfide, γ-mercaptopropyltriethoxysilane, and 3-octanoylthiopropyltriethoxysilane. Among these, those having a tetrasulfide bond in the molecule are particularly suitable. The compounding amount of the silane coupling agent is preferably 3.0% to 10% by mass, more preferably 4.0% to 9.0% by mass, relative to the compounding amount of silica. If the compounding amount of the silane coupling agent is less than 3.0% by mass of the compounding amount of silica, the compounding amount is so small that the effect of compounding the silane coupling agent cannot be fully expected. If the amount of the silane coupling agent exceeds 10% by mass of the amount of silica, the silane coupling agents will condense with each other, making it difficult to obtain the desired hardness and strength in the rubber composition.

[0037] Other compounding agents than those mentioned above can be added to the rubber composition for undertread of the present invention. Examples of other compounding agents include various compounding agents generally used in rubber compositions for tires, such as vulcanizing or crosslinking agents, vulcanization accelerators, antioxidants, and liquid polymers. The compounding amounts of these compounding agents can be conventional amounts as long as they do not contradict the object of the present invention. Furthermore, as the kneading machine, a conventional rubber kneading machine, such as a Banbury mixer, kneader, or roll, can be used.

[0038] As described above, the rubber composition for an undertread of the present invention can be suitably used in the undertread layer of a tire, and a tire having an undertread layer made of the rubber composition for an undertread of the present invention can improve the steering stability and high-speed durability while ensuring good low heat buildup due to the excellent physical properties of the rubber composition for an undertread of the present invention. When the rubber composition for an undertread of the present invention is used in a tire, the tensile stress M100 at 100% elongation at 23°C of the undertread rubber constituting the undertread layer (i.e., the vulcanizate of the rubber composition for an undertread of the present invention) is UT [unit: MPa] and the tensile stress M100 of the side rubber constituting the sidewall portion at 23°C when elongated to 100% SW Ratio M100 [unit: MPa] UT / M100 SW is preferably 1.5 to 4.0, and more preferably 1.8 to 3.5. By optimizing the relationship of the tensile stress (M100) between the undertread layer using the rubber composition for undertread of the present invention and the adjacent sidewall portion (side rubber), it is advantageous to improve the steering stability and high-speed durability while ensuring low heat buildup. UT / M100 SW If the ratio M100 is less than 1.5, the effects of improving low heat buildup, steering stability, and high-speed durability are limited. UT / M100 SW If the value exceeds 4.0, the effects of improving low heat build-up, handling stability and high-speed durability will be limited.

[0039] The present invention will be further explained below with reference to examples, but the scope of the present invention is not limited to these examples.

[0040] The tire size is 245 / 45R18, and has the basic structure shown in FIG. 1. The compounding of the rubber composition for the undertread and the tensile stress (M100) at 100% elongation at 23°C of the undertread rubber and the side rubber are UT , M100 SW ) and its ratio M100 UT / M100 SWTires (test tires) of Standard Example 1, Comparative Examples 1 to 7, and Examples 1 to 8 were manufactured with the values ​​set as shown in Tables 1 and 2.

[0041] Regarding the compounding of the rubber composition for undertread, the compounding common to all examples is summarized in Table 3. Tables 1 and 2 also list the type of side rubber used in each example. The type of side rubber is indicated by the numbers of side rubbers A to B listed in Table 4, and the compounding of these side rubbers A to B is as shown in Table 4.

[0042] The tensile stress (M100 UT , M100 SW ) is a value (unit: MPa) measured using a No. 3 dumbbell test piece prepared in accordance with JIS K6251 using undertread rubber and side rubber at a tensile speed of 500 mm / min and a temperature of 23°C.

[0043] Using each test tire, the steering stability, low rolling resistance, and high-speed durability were evaluated by the methods described below.

[0044] Steering stability Each test tire was mounted on a wheel with a rim size of 18x7J, the air pressure was set to 240 kPa, and the tire was mounted on a test vehicle with an engine displacement of 2000 cc. The test vehicle was then subjected to a sensory evaluation of steering stability by a test driver on a test course consisting of a paved road surface. The evaluation results were evaluated on a 5-point scale, with the result of Standard Example 1 being given 3 points (standard). The higher the score, the better the steering stability.

[0045] Low Rolling Resistance Each test tire was mounted on a wheel with a rim size of 18x7J, and rolling resistance was measured using an indoor drum testing machine (drum diameter: 1707.6 mm) in accordance with ISO 28580 under conditions of an air pressure of 210 kPa, a load of 4.82 kN, and a speed of 80 km / h. The evaluation results were expressed as an index using the reciprocal of the measured value, with Standard Example 1 being 100. The higher the index value, the lower the rolling resistance and the better the low rolling resistance.

[0046] High-Speed ​​Durability Each test tire was mounted on a wheel with a rim size of 18x7J, and a running test was conducted using an indoor drum testing machine (drum diameter: 1707.6 mm) under conditions of an air pressure of 340 kPa, a load of 5 kN, and a negative camber angle of 3°. Specifically, the initial speed was 250 km / h, and the speed was increased by 10 km / h every 20 minutes until the tire failed, and the speed reached was measured. The evaluation results were expressed as an index, with the measured value (speed) of Standard Example 1 being 100. The higher the index value, the greater the speed reached until failure, indicating superior high-speed durability with a camber angle.

[0047]

[0048]

[0049]

[0050] The types of raw materials used in Tables 1 to 3 are shown below. NR: Natural rubber, RSS#3 BR1: Nipol 1220 manufactured by Nippon Zeon Co., Ltd. (butadiene rubber synthesized using a cobalt catalyst, cis-1,4 bond content: 98 mol%, Mw / Mn = 2.9, Tcp / ML 1+4 = 1.4) BR2: Nipol 1250H manufactured by Nippon Zeon Co., Ltd. (butadiene rubber synthesized using a lithium catalyst, cis-1,4 bond content: 35 mol%, Mw / Mn = 1.4) BR3: UBEPOL BR360L manufactured by Ube Industries, Ltd. (butadiene rubber synthesized using a cobalt catalyst, cis-1,4 bond content: 98 mol%, Mw / Mn = 2.2, Tcp / ML 1+4 = 2.8) BR4: Buna CB22 manufactured by ARLANXEO (butadiene rubber synthesized using a neodymium catalyst, cis-1,4 bond content: 98 mol%, Mw / Mn = 2.3, Tcp / ML 1+4 = 6.5) BR5: Buna CB24 manufactured by ARLANXEO (butadiene rubber synthesized using a neodymium catalyst, cis-1,4 bond content: 96 mol%, Mw / Mn = 2.0) CB1: Carbon black (grade: ISAF), SEAT 6 manufactured by Tokai Carbon Co., Ltd. (CTAB adsorption specific surface area: 109 m 2 / g) CB2: Carbon black (grade: HAF), manufactured by Tokai Carbon Co., Ltd., SEAT 3 (CTAB adsorption specific surface area: 82 m 2 / g) CB3: Carbon black (grade: FEF), manufactured by Tokai Carbon Co., Ltd., SEAT F (CTAB adsorption specific surface area: 47 m 2 / g) Silica 1: ULTRASIL VN3GR manufactured by Evonik (CTAB adsorption specific surface area: 175 m 2 / g) Silica 2: ZEOSIL 115GR manufactured by Solvay (CTAB adsorption specific surface area: 115 m 2 / g) Silica 3: Zeosil 1185GR manufactured by Solvay (CTAB adsorption specific surface area: 80 m 2 / g) Silane coupling agent: Si69 manufactured by Evonik Industries AG Stearic acid: Stearic acid 50S manufactured by Nissin Rika Co., Ltd. Zinc oxide: Zinc oxide 3 types manufactured by Seido Chemical Industry Co., Ltd. Antiaging agent: PILFLEX 13 manufactured by NOCIL LIMITED Tackifier: Hitanol 1502Z manufactured by Hitachi Chemical Co., Ltd. Sulfur: Myucron OT-20 manufactured by Shikoku Chemical Industry Co., Ltd. Vulcanization accelerator: Suncerer NS-G manufactured by Sanshin Chemical Industry Co., Ltd.

[0051]

[0052] The types of raw materials used in Table 4 are as follows: NR: Natural rubber, RSS#3 BR: Nipol 1220 manufactured by Nippon Zeon Co., Ltd. CB: Carbon black (grade: FEF), SEAT F manufactured by Tokai Carbon Co., Ltd. (CTAB adsorption specific surface area: 47 m 2 / g) Tackifier: Hitachi Chemical Co., Ltd., Hitanol 1502Z Zinc oxide: Seido Chemical Industry Co., Ltd., zinc oxide 3 types Antioxidant: Nocil Limited, Pilflex 13 Stearic acid: Nissin Rika Co., Ltd., stearic acid 50S Aroma oil: ENEOS Corporation, Aromax T-DAE Sulfur: Tsurumi Chemical Industry Co., Ltd., Sulfax 5 Vulcanization accelerator: Sancerer NS-G

[0053] As is clear from Tables 1 and 2, Examples 1 to 8 improved handling stability, low rolling resistance, and high-speed durability compared to Reference Example 1, achieving a good balance of these performance characteristics. On the other hand, Comparative Example 1 had poor low rolling resistance due to the large CTAB specific surface area of ​​the silica. Comparative Example 2 had poor low rolling resistance due to the large CTAB specific surface area of ​​the silica. Comparative Example 3 had poor high-speed durability due to the use of modified butadiene rubber. Comparative Example 4 had poor high-speed durability due to the low silica content. Comparative Example 5 had poor handling stability due to the high silica content. Comparative Example 6 had poor low rolling resistance due to the high isoprene-based rubber (natural rubber) content and the low unmodified butadiene rubber content. Comparative Example 7 had poor handling stability and high-speed durability due to the low isoprene-based rubber (natural rubber) content and the high unmodified butadiene rubber content.

[0054] REFERENCE SIGNS LIST 1 tread portion 2 sidewall portion 3 bead portion 4 carcass layer 5 bead core 6 bead filler 7 belt layer 8 belt cover layer 10 tread rubber layer 11 cap tread layer 12 under tread layer 20 side rubber layer 30 rim cushion rubber layer CL tire equator

Claims

1. A rubber component having a CTAB adsorption specific surface area of ​​60 m for 100 parts by mass of a rubber component containing 60% by mass to 90% by mass of isoprene-based rubber and 10% by mass to 40% by mass of unmodified butadiene rubber. 2 / g to 100m 2 and a molecular weight distribution (Mw / Mn) calculated from the weight average molecular weight (Mw) and number average molecular weight (Mn) of the unmodified butadiene rubber is 2.8 or less.

2. The CTAB adsorption specific surface area is 40 m for 100 parts by mass of the rubber component. 2 / g ~ 120m 2 2. The rubber composition for undertread according to claim 1, characterized in that 20 to 70 parts by mass of carbon black having a viscosity of 1 / g is blended.

3. The rubber composition for undertread according to claim 1 or 2, characterized in that the unmodified butadiene rubber has a cis-1,4 bond content of 95% or more.

4. The unmodified butadiene rubber has a 5% by mass toluene solution viscosity Tcp (unit: cps) at 25°C and a Mooney viscosity ML at 100°C. 1+4 Ratio of Tcp / ML 1+4 The rubber composition for undertread according to any one of claims 1 to 3, characterized in that the relationship of 5. The rubber composition for undertread according to any one of claims 1 to 4, characterized in that the unmodified butadiene rubber is synthesized using a neodymium-based catalyst.

6. A rubber composition for undertread according to any one of claims 1 to 5, characterized in that a silane coupling agent is blended therein, and the ratio of the blended amount of the silane coupling agent to the blended amount of the silica is 3.0 mass % to 10.0 mass %.

7. A tire comprising a tread portion extending circumferentially in an annular shape and a pair of sidewall portions disposed on either side of the tread portion, the tread portion being constructed by laminating a cap tread layer constituting the tire surface and an undertread layer disposed on its inner side, the undertread layer being constructed from the rubber composition for undertreads according to any one of claims 1 to 6.

8. Tensile stress M100 of the undertread rubber constituting the undertread layer at 100% elongation at 23°C UT [Unit: MPa] and the tensile stress M100 of the side rubber constituting the sidewall portion at 100% elongation at 23°C SW Ratio to M100 [unit: MPa] UT / M100 SW 8. The tire according to claim 7, wherein the tread width is 1.5 to 4.0.

Citation Information

Patent Citations

  • Rubber composition for tire, and pneumatic tire

    JP2012219224A

  • Pneumatic tire

    JP2013177113A

  • Rubber composition for tire

    JP2019026757A

  • Rubber composition for tread, and tire

    JP2019151738A

  • Rubber composition and tire made therefrom

    JP2023069115A