Thread-shaped pressure-sensitive adhesive body
The filamentous adhesive body with a controlled length variation and acrylic adhesive composition addresses the waterproofing deficiency in conventional thread-like adhesives, achieving effective water resistance and adhesive strength for electronic device applications.
Patent Information
- Application Number
- PCT/JP2024/012271
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional thread-like adhesives lack waterproof functionality, particularly in electronic device applications where water resistance is crucial.
A filamentous adhesive body with a multifilament yarn core and an acrylic adhesive, where the standard deviation of the length in the width direction is 100 μm or less, and the adhesive covers 20 to 80% of the core material by mass, providing excellent waterproof properties.
The adhesive body effectively prevents water intrusion into bonded areas, ensuring reliable waterproofing and adhesive strength, even in complex shapes and narrow applications.
Smart Images

Figure JP2024012271_03102024_PF_FP_ABST
Abstract
Description
Thread-like adhesive body
[0001] The present invention relates to a thread-like adhesive material.
[0002] A thread-like adhesive body having a core material and an adhesive is generally formed by coating the adhesive around the core material. For example, Patent Document 1 discloses a thread-like adhesive body having a strong adhesive force and a core material made of four or more multifilaments.
[0003] Such thread-like adhesives are thin and can conform to complex shapes, and therefore can be suitably used in applications where the installation space for the adhesive is limited, such as fixing linear or narrow components in a desired shape, and applications in a variety of fields are possible.
[0004] Japanese Patent Application Publication No. 2020-76066
[0005] In recent years, waterproofing has been required for electronic devices such as mobile phones and smartphones, and waterproofing (waterstopping) has also been required for adhesive threads used to fix components in such applications. However, no study has been conducted on the waterproofing of conventional adhesive threads such as those described in Patent Document 1.
[0006] The present invention has been made in view of the above-mentioned conventional circumstances, and has as its object to provide a thread-like adhesive material that is excellent in waterproofing properties.
[0007] As a result of intensive research into solving the above-mentioned problems, the inventors discovered that the above-mentioned problems can be solved by keeping the variation in the widthwise length of a thread-like adhesive body comprising a core material and an adhesive coating the surface of the core material below a predetermined value, thereby solving the present invention.
[0008] That is, the present invention relates to the following: [1] A thread-like adhesive body comprising a core material and a pressure-sensitive adhesive coating the longitudinal surface of the core material, wherein the standard deviation 3σ of the widthwise length of the thread-like adhesive body calculated by the following method is 100 μm or less, and the core material is a multifilament thread comprising four or more filaments. (Calculation method) The average widthwise length and the standard deviation 3σ of the widthwise length of the thread-like adhesive body are calculated by observing the thread-like adhesive body under a microscope, measuring the widthwise length at 10 points at 1 cm intervals in the longitudinal direction, and calculating the average value and standard deviation 3σ of these values. The widthwise length of the thread-like adhesive body is the maximum value at each measurement point. [2] The thread-like adhesive body according to [1], wherein the amount of adhesion of the pressure-sensitive adhesive is 20 to 80 mass% relative to the core material. [3] The thread-like adhesive body according to [1] or [2], wherein the twist coefficient of the core material is 25 to 120. [4] The thread-like adhesive body according to [1] or [2], wherein the core material is a braided cord. [5] The thread-like adhesive body according to [1] or [2], wherein the pressure-sensitive adhesive comprises a base polymer and a tackifier resin, and the pressure-sensitive adhesive comprises 1 to 100 parts by mass of the tackifier resin per 100 parts by mass of the base polymer. [6] The thread-like adhesive body according to [1] or [2], wherein the pressure-sensitive adhesive is an acrylic pressure-sensitive adhesive.
[0009] According to the present invention, a thread-like adhesive material having excellent waterproof properties can be provided.
[0010] Fig. 1 is a diagram illustrating one example of use of a thread-like adhesive body according to an embodiment of the present invention. Fig. 2 is another diagram illustrating one example of use of a thread-like adhesive body according to an embodiment of the present invention. Fig. 3 is a diagram illustrating a method for evaluating the adhesive strength of a thread-like adhesive body according to an embodiment of the present invention. Fig. 4 is a diagram illustrating a method for evaluating the adhesive strength of a thread-like adhesive body according to an embodiment of the present invention. Fig. 5 is a diagram illustrating a method for evaluating the adhesive strength of a thread-like adhesive body according to an embodiment of the present invention. Fig. 6 is a diagram illustrating a method for evaluating the waterproofness of a thread-like adhesive body according to an embodiment of the present invention. Fig. 7 is another diagram illustrating a method for evaluating the waterproofness of a thread-like adhesive body according to an embodiment of the present invention.
[0011] Hereinafter, embodiments of the thread-like adhesive material of the present invention will be described in detail. Note that the present invention is not limited to the embodiments described below. Furthermore, when the expression "to" is used in this specification, it is used as an expression including the numerical values or physical property values before and after it.
[0012] [Thread-like adhesive body] A thread-like adhesive body according to an embodiment of the present invention is a thread-like adhesive body comprising a core material and an adhesive coating the longitudinal surface of the core material, wherein the standard deviation 3σ of the widthwise length of the thread-like adhesive body calculated by the following method is 100 μm or less, and the core material is a multifilament yarn comprising four or more filaments. (Calculation method) The average widthwise length and standard deviation 3σ of the widthwise length of the thread-like adhesive body are calculated by observing the thread-like adhesive body under a microscope, measuring the widthwise length at 10 points at 1 cm intervals in the longitudinal direction, and calculating the average value and standard deviation 3σ of these values. Note that the widthwise length of the thread-like adhesive body is the maximum value at each measurement point.
[0013] Here, thread-like refers to a shape in which the longitudinal length of the adhesive body is sufficiently long compared to the length in the width direction (direction perpendicular to the longitudinal direction), and the ratio (longest axis / short axis) of the length of the long axis (the longest axis passing through the center of gravity of the cross-sectional shape) to the length of the short axis (the shortest axis passing through the center of gravity of the cross-sectional shape) in the cross-sectional shape (the shape of the cross-section perpendicular to the longitudinal direction) is, for example, 200 or less, preferably 100 or less, more preferably 50 or less, even more preferably 10 or less, still more preferably 5 or less, and particularly preferably 3 or less, and also refers to a shape in which the adhesive body can be bent in various directions and at various angles like a thread.
[0014] The widthwise length of the thread-like adhesive body refers to the length in the thickness direction (direction perpendicular to the longitudinal direction) of the thread-like adhesive body.
[0015] The thread-like adhesive bodies according to the embodiment of the present invention have a widthwise length standard deviation 3σ of 100 μm or less, and exhibit small variations in widthwise length. Therefore, gaps are less likely to occur at the bonded portions between the adherends and the thread-like adhesive bodies. When such thread-like adhesive bodies are used to bond adherends together to produce a bonded structure, water is less likely to penetrate into the spatial region enclosed by the adherends and the thread-like adhesive bodies in the bonded structure.
[0016] Specifically, for example, as shown in Fig. 1, the thread-like adhesive body 1 of this embodiment is placed on the outer periphery of the open surface of a housing 2a having an open surface, with the tip portions overlapping, and the outer periphery of the open surface of another housing 2b is pressed together to produce a joined body 10. Fig. 2 is a schematic cross-sectional view of the joined body 10, and in the joined body 10, water is less likely to penetrate into the region Z surrounded by the housings 2a, 2b and the thread-like adhesive body 1.
[0017] In this specification, the waterproofness of a thread-like adhesive refers to the ability to prevent water from penetrating into the area surrounded by the adherends and the thread-like adhesive in a bonded structure in which adherends are bonded together using the thread-like adhesive.
[0018] Furthermore, since the thread-like adhesive body according to an embodiment of the present invention can be bent in various directions and angles, it can be bent to match the shape of the bonding area, and can accommodate a variety of shapes of bonding areas.
[0019] The core material and adhesive constituting the thread-like adhesive body according to an embodiment of the present invention will be described below.
[0020] <Core Material> The thread-like adhesive material according to the embodiment of the present invention has a core material. The core material is a multifilament yarn having four or more filaments. When the core material is such a multifilament yarn, sufficient strength and stable physical properties can be obtained. As a result, a thread-like adhesive material with low quality variation, excellent strength, and excellent adhesive force can be obtained.
[0021] The number of filaments contained in the core material is 4 or more, and from the viewpoint of adhesive strength, 10 or more is preferable, and 20 or more is more preferable.
[0022] On the other hand, if the thickness (fineness) of the core material is kept at the same level, as the number of filaments increases, each filament becomes thinner (fineness decreases). If each filament becomes too thin, the strength of the core material and handling properties may decrease, so the number of filaments is preferably 2,000 or less, more preferably 1,500 or less, and particularly preferably 1,000 or less.
[0023] There are no particular limitations on the type of resin used for the filament, and it may be selected appropriately depending on the required properties such as strength, mass, hardness, etc. Examples include materials containing polymeric materials such as thermoplastic polymers, thermosetting polymers, and rubber.
[0024] Specifically, polymeric materials such as rayon, cupra, acetate, promix, nylon, aramid, vinylon, vinylidene, polyvinyl chloride, acrylic, polyolefin (polyethylene, polypropylene, ethylene-propylene copolymer, ethylene-vinyl acetate copolymer, etc.), polyester resin (polyethylene terephthalate, etc.), vinyl chloride resin, vinyl acetate resin, polyimide resin, polyamide resin, fluororesin, polyurethane, polychlor, polylactic acid, etc.; rubbers such as synthetic rubber (natural rubber, polyurethane, etc.); foams such as polyurethane foam and polychloroprene rubber foam, etc. can be used. Among these, polyester resin is preferred, and polyethylene terephthalate is more preferred.
[0025] The content of the filaments in the core material is preferably from 10 to 100% by mass, more preferably from 50 to 100% by mass, and particularly preferably from 80 to 100% by mass.
[0026] The core material may contain various additives, such as fillers (inorganic fillers, organic fillers, etc.), antioxidants, antioxidants, ultraviolet absorbers, antistatic agents, lubricants, plasticizers, colorants (pigments, dyes, etc.), etc. The surface of the core material may be subjected to known or conventional surface treatments, such as corona discharge treatment, plasma treatment, or application of a primer.
[0027] The shape of the core material is not particularly limited and may be adjusted appropriately depending on the required properties such as strength, mass, hardness, etc. The cross-sectional shape of the core material is typically circular, but may also be various other shapes such as oval or polygonal as long as waterproofing is ensured.
[0028] The core material may be a non-twisted multifilament yarn made by doubling four or more filaments, or may be a twisted multifilament yarn.
[0029] The core material may have four or more filaments, and may be a yarn obtained by twisting or otherwise combining a filament with a spun yarn, textured yarn, hollow yarn, etc. Examples of textured yarn include textured yarns that have been subjected to crimping or bulking processes and are generally called textured yarns, bulky yarns, and stretch yarns.
[0030] The thickness of the core material is not particularly limited and may be adjusted appropriately depending on the application so that the thickness of the thread-like adhesive body is appropriate, but may be, for example, 200 μm or more, or 500 μm or more, or 200 μm or less, or 100 μm or less.
[0031] In an embodiment of the present invention, the core material may be either twisted or untwisted as described above, but one preferred embodiment is to use a twisted multifilament yarn as the core material. When the core material is twisted, the twist number of the core material is preferably 70 times / m or more. A twist number of 70 times / m or more reduces variation in the diameter (widthwise length) of the core material and can suppress variation in the widthwise length of the resulting filamentous adhesive body. The twist number of the core material is more preferably 80 times / m or more, and even more preferably 90 times / m or more.
[0032] On the other hand, in order to ensure that the core material is sufficiently deformed when multiple articles are bonded together and to appropriately increase the amount of adhesive attached per unit length, it is preferable that the twist of the core material is not too strong. Therefore, the number of twists of the core material is preferably 500 times / m or less, more preferably 300 times / m or less, and even more preferably 200 times / m or less.
[0033] Furthermore, when the core material is twisted, it is preferable to also control the twist coefficient K, which is expressed by the following formula (A), from the same viewpoint as above. The twist coefficient K is an index for discussing the influence of twist (influence on the core material's cohesion, ease of deformation, amount of adhesive attached, etc.) regardless of the thickness of the core material. In other words, the influence of the number of twists on the core material differs depending on the thickness of the core material, but if the twist coefficient K is the same, it indicates that the influence of twist on the core material is the same regardless of the thickness of the core material.
[0034] The twist coefficient K is preferably 24 or more, more preferably 25 or more, and even more preferably 31 or more, from the viewpoint of reducing the variation in the diameter of the core material and suppressing the variation in the width direction length of the resulting thread-like adhesive body. On the other hand, if the twist coefficient K is 120 or less, the flexibility of the core material, and therefore the thread-like adhesive body, is improved, making it easier to apply to complex shapes such as curved portions, bent portions, and uneven portions, or narrow areas. In addition, the amount of adhesive attached per unit length can be appropriately increased. Therefore, the twist coefficient K is preferably 120 or less, more preferably 100 or less, and even more preferably 80 or less. In the thread-like adhesive body according to the embodiment of the present invention, the twist coefficient of the core material is preferably 25 to 120.
[0035]
[0036] In formula (A), K represents the twist coefficient, T represents the number of twists (turns / m), and D represents the fineness (dtex).
[0037] In an embodiment of the present invention, a preferred embodiment is one in which the core material is a braided cord. In this specification, a braided cord is a cord-like material formed by braiding multiple threads, and refers to a cord-like material in which multiple threads are regularly woven. Such a braided cord has small variation in diameter (length in the width direction). Therefore, by using a braided cord as the core material, variation in the diameter of the core material can be reduced, and variation in the length in the width direction of the resulting thread-like adhesive body can be suppressed. The braided cord may be formed by braiding multiple twisted yarns or non-twisted yarns.
[0038] In an embodiment of the present invention, from the viewpoint of variation in the length of the core material in the width direction, the number of ends of the braid is preferably 4 or more, more preferably 5 or more, and particularly preferably 6 or more. Moreover, from the viewpoint of the degree of impregnation of the adhesive into the thread-like adhesive body, the number of ends of the braid is preferably 100 or less, more preferably 95 or less, and particularly preferably 90 or less.
[0039] The content of the core material in the thread-like adhesive is preferably 10% by mass or more, more preferably 20% by mass or more, and particularly preferably 30% by mass or more, from the viewpoint of suppressing a decrease in the strength of the thread-like adhesive, and is preferably 90% by mass or less, more preferably 80% by mass or less, and particularly preferably 70% by mass or less, from the viewpoint of suppressing the core material from coming out to the surface.
[0040] <Adhesive> The thread-like adhesive body according to an embodiment of the present invention has an adhesive that coats a core material. The adhesive in this embodiment can be formed from an adhesive composition, and the adhesive may be an adhesive composition. Furthermore, the adhesive may form a layer (adhesive layer).
[0041] The adhesive preferably covers the entire longitudinal surface of the core material. The entire longitudinal surface of the core material refers to the entire circumferential surface of the core material, and means the entire 360° circumference of the surface of the core material, centered on the center line of the longitudinal direction of the core material.
[0042] However, the end faces of the core material may or may not be coated with adhesive. For example, if the thread-like adhesive body is cut during production or use, the end faces of the core material may not be coated with adhesive.
[0043] By coating the entire longitudinal surface of the core material with an adhesive, a thread-like adhesive body with excellent strength can be obtained. This is thought to be because the core material is not exposed on the surface, preventing stress from concentrating on one part of the core material and causing breakage. Furthermore, by coating the entire longitudinal surface of the core material with an adhesive, gaps are less likely to occur at the bonded portion between the thread-like adhesive body and the adherend, resulting in a thread-like adhesive body with excellent waterproofing.
[0044] The adhesive forming the adhesive layer may be impregnated into the core material. Here, "the adhesive is impregnated into the core material" means that the adhesive is present between multiple filaments in the core material. When the adhesive is impregnated into the core material, the adhesive and the core material maintain adhesion, making them less likely to peel off, and improving the strength of the thread-like adhesive body.
[0045] The adhesive in this embodiment is preferably formed from an adhesive containing a base polymer as a main component. The type of adhesive is not particularly limited, and examples thereof include acrylic adhesives, rubber adhesives, vinyl alkyl ether adhesives, silicone adhesives, polyester adhesives, polyamide adhesives, urethane adhesives, fluorine adhesives, and epoxy adhesives.
[0046] Among these, from the viewpoint of adhesiveness, acrylic adhesives and rubber adhesives are preferred, and acrylic adhesives are more preferred. Note that the adhesives may be used alone or in combination of two or more. In this embodiment, the adhesive is preferably an acrylic adhesive.
[0047] The rubber-based adhesive is based on a rubber-based polymer such as natural rubber, styrene-isoprene-styrene block copolymer, styrene-butadiene-styrene block copolymer, styrene-ethylene-butylene-styrene block copolymer, styrene-butadiene rubber, polybutadiene, polyisoprene, polyisobutylene, butyl rubber, chloroprene rubber, or silicone rubber.
[0048] Here, "acrylic pressure-sensitive adhesive" refers to a pressure-sensitive adhesive having an acrylic polymer as the base polymer (the main component of the polymer, i.e., a component accounting for 50% by mass or more). "Acrylic polymer" refers to a polymer having a monomer having at least one (meth)acryloyl group in one molecule (hereinafter, this may be referred to as "acrylic monomer") as the main constituent monomer component (the main component of the monomer, i.e., a component accounting for more than 50% by mass of the total amount of monomers constituting the acrylic polymer). Furthermore, in this specification, "(meth)acryloyl" refers to acryloyl and methacryloyl in a comprehensive sense. Similarly, "(meth)acrylic acid ester" refers to acrylic acid ester and methacrylic acid ester, and "(meth)acrylic" refers to acrylic and methacrylic in a comprehensive sense.
[0049] The acrylic polymer is preferably a polymer of a monomer raw material that contains, for example, an alkyl(meth)acrylate as a main monomer and may further contain a secondary monomer copolymerizable with the main monomer, where the main monomer refers to a component that accounts for more than 50% by mass of the monomer composition in the monomer raw material.
[0050] As the alkyl(meth)acrylate, for example, a compound represented by the following formula (1) can be suitably used: CH 2 = C(R 1 ) COOR 2 (1) Here, R in the above formula (1) 1 is a hydrogen atom or a methyl group. 2 is a chain alkyl group having 1 to 20 carbon atoms. Hereinafter, this range of carbon atoms will be referred to as "C 1-20 " is sometimes expressed as ".
[0051] R 2 is C 1-20Examples of alkyl(meth)acrylates, which are chain alkyl groups, include methyl(meth)acrylate, ethyl(meth)acrylate, propyl(meth)acrylate, isopropyl(meth)acrylate, n-butyl(meth)acrylate, isobutyl(meth)acrylate, s-butyl(meth)acrylate, pentyl(meth)acrylate, isopentyl(meth)acrylate, hexyl(meth)acrylate, heptyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, octyl(meth)acrylate, and isooctyl(meth)acrylate. Examples of alkyl (meth)acrylates include methyl (meth)acrylate, ...
[0052] From the viewpoint of adhesive stability, etc., R 2 is C 1-14 (For example, C 2-10 , typically C 4-8 It is suitable to use alkyl (meth)acrylate, which is a chain alkyl group of the formula (I), as the main monomer.
[0053] From the viewpoint of adhesive properties, R 1 is a hydrogen atom and R 2 is C 4-8 alkyl acrylate (hereinafter simply referred to as C 4-8 It is preferable to use alkyl acrylates (also called alkyl acrylates) as the main monomer. Preferred examples include n-butyl acrylate (BA) and 2-ethylhexyl acrylate (2EHA).
[0054] That is, the PSA contains an acrylic polymer, and the amount of n-butyl acrylate or 2-ethylhexyl acrylate relative to the total amount of the monomer components constituting the acrylic polymer is preferably more than 50% by mass, more preferably 60% by mass or more, and even more preferably 70% by mass or more. From the viewpoint of suppressing a decrease in adhesive strength, it is preferably 97% by mass or less, more preferably 95% by mass or less, and even more preferably 90% by mass or less.
[0055] In this embodiment, C is used relative to the total amount of monomer components constituting the acrylic polymer. 4-8 The composition can be preferably implemented in an embodiment in which the total amount of alkyl acrylate is more than 50% by mass, and may be 60% by mass or more, 70% by mass or more, or 85% by mass or more. On the other hand, from the viewpoint of cohesive strength, etc., the proportion of C in the monomer components is preferably 100% by mass or more. 4-8 The proportion of alkyl acrylate is usually suitably 99.5% by mass or less, and may be 98% by mass or less (for example, less than 97% by mass).
[0056] The total amount of alkyl(meth)acrylate relative to the total amount of monomer components constituting the acrylic polymer is typically more than 50% by mass, and can be, for example, 70% by mass or more, or 85% by mass or more, or even 90% by mass or more. The proportion of alkyl(meth)acrylate in the monomer components is typically less than 100% by mass, and from the viewpoint of cohesive strength, etc., it is usually appropriate to set it to 99.5% by mass or less, and it may be 98% by mass or less (for example, less than 97% by mass).
[0057] In another preferred embodiment, the adhesive composition contains at least one selected from the group consisting of an alkyl(meth)acrylate having a linear alkyl group having 1 to 3 carbon atoms, an alkyl(meth)acrylate having a branched alkyl group having 3 or 4 carbon atoms, and an alicyclic monomer. That is, it is also preferred that the adhesive composition forming the adhesive contains an acrylic polymer, and that the acrylic polymer contains, as a monomer component, at least one selected from the group consisting of an alkyl(meth)acrylate having a linear alkyl group having 1 to 3 carbon atoms, an alkyl(meth)acrylate having a branched alkyl group having 3 or 4 carbon atoms, and an alicyclic monomer.
[0058] Homopolymers of these monomers have relatively high Tg, and hereinafter these monomers are also referred to as high Tg monomers.
[0059] The alicyclic monomer is preferably a cycloalkyl(meth)acrylate having a cycloalkyl group having 4 to 10 carbon atoms which may have a substituent (for example, a linear or branched alkyl group having 1 to 6 carbon atoms), more preferably a cycloalkyl acrylate having a cycloalkyl group having 4 to 10 carbon atoms which may have a substituent (for example, a linear or branched alkyl group having 1 to 6 carbon atoms), and particularly preferably cyclohexyl acrylate or 3,3,5-trimethylcyclohexyl (meth)acrylate.
[0060] As the alkyl (meth)acrylate having a linear alkyl group with 1 to 3 carbon atoms, an alkyl acrylate having a linear alkyl group with 1 to 3 carbon atoms is preferred, and methyl acrylate is particularly preferred.
[0061] As the alkyl (meth)acrylate having a branched alkyl group with 3 or 4 carbon atoms, an alkyl acrylate having a branched alkyl group with 3 or 4 carbon atoms is preferred, and t-butyl acrylate is particularly preferred.
[0062] Among them, the high Tg monomer is preferably an alkyl acrylate having a linear alkyl group with 1 to 3 carbon atoms, and methyl acrylate is particularly preferred.
[0063] In an embodiment in which a high Tg monomer is copolymerized with an acrylic polymer, the total amount of the high Tg monomer relative to the total amount of the monomer components constituting the acrylic polymer is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more. Furthermore, from the viewpoint of suppressing a decrease in the adhesive strength of the PSA, it is preferably 20% by mass or less, more preferably 18% by mass or less, and even more preferably 15% by mass or less. That is, the total amount of at least one monomer selected from the group consisting of alkyl(meth)acrylates having a linear alkyl group with 1 to 3 carbon atoms, alkyl(meth)acrylates having a branched alkyl group with 3 or 4 carbon atoms, and alicyclic monomers is preferably 1 to 20% by mass relative to the total amount of the monomer components constituting the acrylic polymer.
[0064] The acrylic polymer may contain a carboxyl group-containing monomer as a monomer component constituting the acrylic polymer. Examples of the carboxyl group-containing monomer include ethylenically unsaturated monocarboxylic acids such as acrylic acid, methacrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, crotonic acid, and isocrotonic acid; ethylenically unsaturated dicarboxylic acids such as maleic acid, itaconic acid, and citraconic acid, and their anhydrides (maleic anhydride, itaconic anhydride, etc.); and the like. These can be used alone or in combination of two. Among them, acrylic acid (AA) and methacrylic acid (MAA) are preferred as carboxyl group-containing monomers. AA is particularly preferred.
[0065] In an embodiment in which a carboxyl group-containing monomer is copolymerized with an acrylic polymer, the content of the carboxyl group-containing monomer relative to the total amount of the monomer components constituting the acrylic polymer is not particularly limited, and can be, for example, 0.2% by mass or more (typically 0.5% by mass or more), and usually 1% by mass or more is appropriate, and may be 2% by mass or more, or 3% by mass or more. The upper limit of the content of the carboxyl group-containing monomer is not particularly limited, but from the viewpoint of maintaining good adhesive properties, it can be, for example, 15% by mass or less, or may be 12% by mass or less, or may be 10% by mass or less.
[0066] The acrylic polymer may be formed using, as a monomer component, one or more of the following functional group-containing monomers (excluding the above-mentioned carboxy group-containing monomers): Hydroxyl group-containing monomers: hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; unsaturated alcohols such as vinyl alcohol and allyl alcohol; and polypropylene glycol mono(meth)acrylate. Amide group-containing monomers: (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N-butyl (meth)acrylamide, N-methylol (meth)acrylamide, N-methylolpropane (meth)acrylamide, N-methoxymethyl (meth)acrylamide, and N-butoxymethyl (meth)acrylamide. Amino group-containing monomers: for example, aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, t-butylaminoethyl (meth)acrylate. Epoxy group-containing monomers: for example, glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, allyl glycidyl ether. Cyano group-containing monomers: for example, acrylonitrile, methacrylonitrile. Keto group-containing monomers: for example, diacetone (meth)acrylamide, diacetone (meth)acrylate, vinyl methyl ketone, vinyl ethyl ketone, allyl acetoacetate, vinyl acetoacetate. Monomers having a nitrogen atom-containing ring: for example, N-vinyl-2-pyrrolidone, N-methylvinylpyrrolidone, N-vinylpyridine, N-vinylpiperidone, N-vinylpyrimidine, N-vinylpiperazine, N-vinylpyrazine, N-vinylpyrrole, N-vinylimidazole, N-vinyloxazole, N-vinylmorpholine, N-vinylcaprolactam, and N-(meth)acryloylmorpholine.
[0067] When the monomer component constituting the acrylic polymer contains the functional group-containing monomer described above, the content of the functional group-containing monomer in the monomer component is not particularly limited. From the viewpoint of properly achieving the effects of using the functional group-containing monomer, the content of the functional group-containing monomer in the monomer component can be, for example, 0.1% by mass or more, typically 0.5% by mass or more, and may be 1% by mass or more. Furthermore, from the viewpoint of easily balancing the adhesive performance, typically 40% by mass or less is suitable, preferably 20% by mass or less, and may be 10% by mass or less (e.g., 5% by mass or less). The technology disclosed herein can also be preferably implemented in an embodiment in which the monomer component is substantially free of functional group-containing monomers (e.g., an embodiment in which the monomer component is substantially composed only of alkyl (meth)acrylate and carboxy group-containing monomer). Here, "substantially free of functional group-containing monomers" means that functional group-containing monomers are not used at least intentionally, and for example, the unintentional inclusion of functional group-containing monomers at 0.05% by mass or less (typically 0.01% by mass or less) is acceptable.
[0068] The monomer components constituting the acrylic polymer may contain copolymerization components other than the above-mentioned monomers. Examples of the copolymerization components include vinyl ester monomers such as vinyl acetate, vinyl propionate, and vinyl laurate; aromatic vinyl compounds such as styrene, substituted styrenes (α-methylstyrene, etc.), and vinyltoluene; cycloalkyl(meth)acrylates such as cyclohexyl(meth)acrylate, cyclopentyl(meth)acrylate, and isobornyl(meth)acrylate; and aromatic ring-containing (meth)acrylates such as aryl(meth)acrylates (e.g., phenyl(meth)acrylate), aryloxyalkyl(meth)acrylates (e.g., phenoxyethyl(meth)acrylate), and arylalkyl(meth)acrylates (e.g., benzyl(meth)acrylate). olefin-based monomers such as ethylene, propylene, isoprene, butadiene, and isobutylene; chlorine-containing monomers such as vinyl chloride and vinylidene chloride; isocyanate group-containing monomers such as 2-(meth)acryloyloxyethyl isocyanate; alkoxy group-containing monomers such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate; vinyl ether-based monomers such as methyl vinyl ether and ethyl vinyl ether; polyfunctional monomers having two or more (e.g., three or more) polymerizable functional groups (e.g., (meth)acryloyl groups) in one molecule, such as 1,6-hexanediol di(meth)acrylate and trimethylolpropane tri(meth)acrylate; and the like.
[0069] The amount of such other copolymerization components can be appropriately selected depending on the purpose and application, and is not particularly limited. From the viewpoint of properly exerting the effects of use, it is usually appropriate to set it to 0.05% by mass or more, and it may be 0.5% by mass or more. Furthermore, from the viewpoint of easily balancing adhesive performance, the content of other copolymerization components in the monomer component is usually appropriate to set it to 20% by mass or less, and it may be 10% by mass or less (e.g., 5% by mass or less). In this embodiment, an embodiment in which the monomer component is substantially free of other copolymerization components can also be preferably implemented. Here, "substantially free of other copolymerization components" means that other copolymerization components are not used at least intentionally, and it is acceptable for other copolymerization components to be unintentionally included, for example, at 0.01% by mass or less.
[0070] The adhesive may also contain various additives, such as a tackifying resin, a crosslinking agent, a viscosity modifier (such as a thickener), a leveling agent, a release modifier, a plasticizer, a softener, a filler, a colorant (such as a pigment or dye), a surfactant, an antistatic agent, a preservative, an antioxidant, an ultraviolet absorber, an antioxidant, and a light stabilizer, as appropriate.
[0071] It is preferable to blend a crosslinking agent into the acrylic pressure-sensitive adhesive. The crosslinking agent used in the acrylic pressure-sensitive adhesive can be a commonly used crosslinking agent, such as a silane-based crosslinking agent, an organic peroxide, an epoxy-based compound, an amino group-containing compound, an organic metal salt, a metal alcoholate, a metal chelate, a hydrazide-based crosslinking agent, a carbodiimide-based crosslinking agent, an isocyanate-based crosslinking agent, or a silanol-based crosslinking agent. Among these, organic metal salts, metal chelates, hydrazide-based crosslinking agents, and silane-based crosslinking agents are preferred because they rapidly complete crosslinking after the pressure-sensitive adhesive composition is dried. In the case of a water-dispersible pressure-sensitive adhesive, hydrazide-based crosslinking agents and silane-based crosslinking agents are particularly preferred. The crosslinking agent may be either oil-soluble or water-soluble, and may be used alone or in combination of two or more.
[0072] As the silane crosslinking agent, it is preferable to use a silane monomer copolymerizable with the (meth)acrylic acid alkyl ester. The silane monomer is not particularly limited as long as it is a polymerizable compound having a silicon atom. However, silane compounds having a (meth)acryloyl group, such as (meth)acryloyloxyalkylsilane derivatives, are preferred because of their excellent copolymerizability with the (meth)acrylic acid alkyl ester. Examples of silane monomers include γ-methacryloxypropyltrimethoxysilane, 3-acryloyloxypropyltrimethoxysilane, 3-methacryloyloxypropyltriethoxysilane, 3-acryloyloxypropyltriethoxysilane, 3-methacryloyloxypropylmethyldimethoxysilane, 3-acryloyloxypropylmethyldimethoxysilane, 3-methacryloyloxypropylmethyldiethoxysilane, and 3-acryloyloxypropylmethyldiethoxysilane. These silane monomers can be used alone or in combination of two or more.
[0073] In addition to the above, examples of copolymerizable silane monomers that can be used include vinyltrimethoxysilane, vinyltriethoxysilane, 4-vinylbutyltrimethoxysilane, 4-vinylbutyltriethoxysilane, 8-vinyloctyltrimethoxysilane, 8-vinyloctyltriethoxysilane, 10-methacryloyloxydecyltrimethoxysilane, 10-acryloyloxydecyltrimethoxysilane, 10-methacryloyloxydecyltriethoxysilane, and 10-acryloyloxydecyltriethoxysilane.
[0074] The amount of the crosslinking agent used can be appropriately selected depending on the type of the monomer raw material, the application of the adhesive article, etc. In this embodiment, the amount of the crosslinking agent relative to 100 parts by mass of the monomer raw material (excluding the crosslinking agent) is preferably 0.005 to 5 parts by mass, and more preferably 0.01 to 3 parts by mass.
[0075] In this embodiment, other crosslinking agents may also be used, and crosslinking using other crosslinking agents, UV crosslinking, radiation crosslinking such as electron beam crosslinking, etc. may be applied. As the other crosslinking agent, a commonly used crosslinking agent may be used, and examples thereof include organic peroxides, epoxy compounds, amino group-containing compounds, organic metal salts, metal alcoholates, metal chelates, hydrazide crosslinking agents, carbodiimide crosslinking agents, isocyanate crosslinking agents, and silane or silanol crosslinking agents. The other crosslinking agent may be either oil-soluble or water-soluble.
[0076] The pressure-sensitive adhesive according to the present embodiment may preferably use a tackifying resin. Any appropriate tackifying resin may be used as the tackifying resin. Specific examples of tackifying resins include rosin-based tackifying resins (e.g., unmodified rosin, modified rosin, rosin phenolic resins, rosin ester resins, etc.), terpene-based tackifying resins (e.g., terpene resins, terpene phenolic resins, styrene-modified terpene resins, aromatic-modified terpene resins, hydrogenated terpene resins), hydrocarbon-based tackifying resins (e.g., aliphatic hydrocarbon resins, aliphatic cyclic hydrocarbon resins, aromatic hydrocarbon resins (e.g., styrene-based resins, xylene-based resins, etc.), aliphatic / aromatic petroleum resins, aliphatic / alicyclic petroleum resins, hydrogenated hydrocarbon resins, coumarone-based resins, coumarone-indene resins, etc.), phenol-based tackifying resins (e.g., alkylphenol-based resins, xylene-formaldehyde-based resins, resols, novolacs, etc.), ketone-based tackifying resins, polyamide-based tackifying resins, epoxy-based tackifying resins, and elastomer-based tackifying resins. Among these, rosin-based tackifying resins, terpene-based tackifying resins, and hydrocarbon-based tackifying resins (such as styrene-based resins) are preferred. The tackifying resins may be used alone or in combination of two or more.
[0077] In an embodiment in which the PSA contains a tackifier resin, the amount of the tackifier resin added is preferably 1 part by mass or more, more preferably 10 parts by mass or more, even more preferably 20 parts by mass or more, and even more preferably 30 parts by mass or more, relative to 100 parts by mass of the base polymer. From the viewpoint of suppressing a decrease in the adhesive strength of the PSA, the amount is preferably 100 parts by mass or less, more preferably 90 parts by mass or less, and even more preferably 70 parts by mass or less.
[0078] The adhesive composition that forms the adhesive contains a base polymer and a tackifier resin, and preferably contains 1 to 100 parts by mass of the tackifier resin per 100 parts by mass of the base polymer.
[0079] The PSA composition may be either a solvent-based PSA or a water-dispersed PSA. A water-dispersed PSA composition is preferred because it allows high-speed coating, is environmentally friendly, and minimizes the impact of the solvent on the core material (swelling, dissolution). In an embodiment of the present invention, the PSA is preferably an acrylic emulsion PSA containing a water-dispersed acrylic polymer.
[0080] Specifically, the adhesive amount (mass of adhesive per unit length) is preferably 2 mg / m or more, more preferably 5 mg / m or more, and even more preferably 8 mg / m or more. On the other hand, if the adhesive amount is excessive, the adhesive composition needs to be applied to the core material multiple times in the manufacturing process, and the applied adhesive composition takes a long time to dry, resulting in low manufacturing efficiency. Therefore, the adhesive amount is preferably 200 mg / m or less, more preferably 180 mg / m or less, and even more preferably 160 mg / m or less.
[0081] The amount of adhesive attached is preferably 10% by mass or more, more preferably 20% by mass or more, and particularly preferably 30% by mass or more, relative to the core material, from the viewpoints of ensuring waterproofness and adhesive strength. Furthermore, from the viewpoints of suppressing variation in the width direction length of the thread-like adhesive bodies and suppressing a decrease in the strength of the thread-like adhesive bodies, the amount is preferably 90% by mass or less, more preferably 80% by mass or less, and particularly preferably 70% by mass or less. In this embodiment, the amount of adhesive attached is preferably 20 to 80% by mass relative to the core material.
[0082] From the viewpoints of strength and handleability, the width of the thread-like adhesive body according to the embodiment of the present invention is preferably 50 μm or more, more preferably 100 μm or more, and is preferably 2000 μm or less, more preferably 1000 μm or less.
[0083] The standard deviation 3σ of the widthwise length of the thread-like adhesive body according to an embodiment of the present invention is 100 μm or less. By using a thread-like adhesive body with a small variation in widthwise length (3σ of 100 μm or less), gaps are less likely to occur in the bonded portion between the adherend and the thread-like adhesive body, and therefore, in a bonded body in which adherends are bonded together by the thread-like adhesive body according to an embodiment of the present invention, water is less likely to penetrate into the area surrounded by the adherend and the thread-like adhesive body.
[0084] 3σ is 100 μm or less, and from the viewpoint of improving waterproofness, it is preferably 80 μm or less, more preferably 60 μm or less. The lower limit of 3σ is 0 μm, but from the viewpoint of productivity, it is preferably 5 μm or more, more preferably 10 μm or more.
[0085] As described above, in this embodiment, the average width length of the thread-like adhesive bodies and the standard deviation 3σ of the width length are values calculated by observing the thread-like adhesive bodies with a microscope, measuring the width length at 10 points at intervals of 1 cm in the longitudinal direction, and calculating the average value and standard deviation 3σ of these values. Note that the width length of the thread-like adhesive bodies is the maximum value at each measurement point.
[0086] Specifically, first, a ruler is placed on the stage of the microscope and the scale is calibrated. Then, the adhesive filaments are placed and their position is finely adjusted so that the latitude lines of the grid-like scale displayed on the observation screen are parallel to the long axis of the adhesive filaments. Next, the observation magnification of the microscope is set to 30 times, and the length of the short axis (length in the width direction) of the adhesive filaments is measured at 10 points at 1 cm intervals in the longitudinal direction. The obtained measurement values (X 1 , X 2 ,...,X 10 ) is used to calculate the average value m (average value of the length of the thread-like adhesive bodies in the width direction). Then, the standard deviation 3σ (μm) is calculated using the following formula (4).
[0087]
[0088] In formula (4), X 1 , X 2 ,...,X n represents each measured value, m represents the average value, and n represents the number of data. In the measurement method of this embodiment, n is 10.
[0089] [Method for producing thread-like adhesive body] The thread-like adhesive body according to the embodiment of the present invention can be produced by a known method, for example, a method including a coating step of coating a core material with a coating liquid containing an adhesive. The coating of the coating liquid may be carried out once or multiple times.
[0090] The coating liquid may be applied to the core material by, for example, dipping, immersion, coating, or the like, and may be dried by heating as necessary. The drying by heating may be carried out, for example, at a temperature of 80 to 120°C, preferably 90 to 110°C, for a period of 20 seconds to 3 minutes, preferably 30 seconds to 2 minutes.
[0091] The coating liquid can be applied using a conventional coater such as a gravure roll coater, a reverse roll coater, a kiss roll coater, a dip roll coater, a bar coater, a knife coater, or a spray coater.
[0092] The method for producing a thread-like adhesive body of this embodiment may or may not include a fiber-spreading step. In the fiber-spreading step, the core material is spread by running the core material along a non-rotating roller when the adhesive is applied to the core material. When the thread-like adhesive body of this embodiment is produced without a fiber-spreading step, the porosity in the thread-like adhesive body can be adjusted to be high. On the other hand, when the thread-like adhesive body of this embodiment is produced with a fiber-spreading step, the porosity in the thread-like adhesive body can be adjusted to be low.
[0093] Furthermore, when the method for producing a thread-like adhesive body of this embodiment includes a coating step, the coating step uses a roller, and the rotation speed of the roller is preferably 0.3 to 5.0 times the payout speed of the core material, more preferably 0.4 to 4.0 times, even more preferably 0.5 to 3.0 times, and particularly preferably 0.8 to 1.5 times the payout speed of the core material.
[0094] In the coating step, it is preferable to apply a tension of 6.0 mN / dtex or less to the core material, preferably 0.2 to 6.0 mN / dtex, more preferably 0.4 to 5.0 mN / dtex.
[0095] One preferred aspect of the thread-like adhesive body according to an embodiment of the present invention is that it includes, after the coating step, a threading step in which the core material coated with the coating liquid is threaded through a cylindrical or comb-shaped gap.
[0096] A method for producing a thread-like adhesive body according to one embodiment of the present invention is a method for producing a thread-like adhesive body comprising a core material and an adhesive that coats the longitudinal surface of the core material, and includes a coating process of coating the core material with a coating liquid containing the adhesive, and a threading process of threading the core material coated with the coating liquid through a cylindrical or comb-shaped gap, wherein the standard deviation 3σ of the width direction length of the thread-like adhesive body is 100 μm or less, and the core material is a multifilament yarn having four or more filaments.
[0097] For example, when a coating liquid is applied to a core material by dipping, the amount of coating liquid adhered to the core material may be relatively large, and the amount of coating liquid adhering to the core material may become uneven due to the influence of gravity during transport, adhesion to the rollers used, etc. Therefore, by threading the core material coated with the coating liquid through a cylindrical or comb-shaped gap having a certain inner diameter, the unevenly adhered coating liquid can be leveled out, and variation in the width direction length of the resulting thread-like adhesive body can be suppressed.
[0098] [Uses of adhesive threads] The adhesive threads according to the embodiments of the present invention have excellent waterproof properties, and therefore can be used to adhere articles that require waterproofing and sealing properties. For example, in the manufacture of electronic devices, adhesive threads according to the embodiments of the present invention can be used to prevent water from entering into a housing (e.g., housing 2a in FIG. 1 ) containing components that should be prevented from entering into water, such as a battery or a circuit board, by adhering the housing to another member (e.g., housing 2b in FIG. 1 ).
[0099] Furthermore, the adhesive thread according to the embodiment of the present invention can be attached to narrow members or narrow areas while preventing overhang, and is easily applicable to complex shapes such as curves, curved surfaces, and uneven surfaces, and is also preferable in that it can be easily disassembled (reworked). Furthermore, due to its excellent adhesive strength, it can be used to adhere various items.
[0100] Furthermore, for example, when applying an adhesive tape to an adherend having a complex shape, such as a curve, a curved surface, or an uneven surface, wrinkles and overlaps may occur in the adhesive tape in those areas, making it difficult to apply the tape neatly while preventing overhang. Furthermore, the wrinkles and overlaps may also cause a decrease in waterproofness and adhesive strength. To apply an adhesive tape without wrinkles or overlaps, it is possible to cut the adhesive tape into small pieces before application, but this significantly reduces workability and makes it difficult to achieve the desired waterproofness. On the other hand, the adhesive thread according to the embodiment of the present invention can be firmly applied without wrinkles or overlaps, even when applied to a complex shape, such as a curve, a curved surface, or an uneven surface, and can exhibit excellent waterproofness. Furthermore, since such adhesive threads can be applied to the desired areas at once, i.e., in a single process, they are easy to work with and can be applied to automated lines.
[0101] Furthermore, the thread-like adhesive material according to the embodiment of the present invention can be suitably used for the purpose of temporarily fixing (temporarily fastening) one article to the surface of another article. Furthermore, with the thread-like adhesive material according to the embodiment of the present invention, after the two articles have been fixed (fully fixed), it is easy to remove the thread-like adhesive material according to the embodiment of the present invention from between the two fixed (fully fixed) articles, as needed.
[0102] As explained above, the present specification discloses the following. [1] A thread-like adhesive body comprising a core material and a pressure-sensitive adhesive coating the longitudinal surface of the core material, wherein the standard deviation 3σ of the widthwise length of the thread-like adhesive body calculated by the following method is 100 μm or less, and the core material is a multifilament thread comprising four or more filaments. (Calculation method) The average widthwise length and the standard deviation 3σ of the widthwise length of the thread-like adhesive body are calculated by observing the thread-like adhesive body with a microscope, measuring the widthwise length at 10 points at 1 cm intervals in the longitudinal direction, and calculating the average value and standard deviation 3σ of these values. The widthwise length of the thread-like adhesive body is the maximum value at each measurement point. [2] The thread-like adhesive body according to [1], wherein the amount of adhesive attached is 20 to 80 mass% of the core material. [3] The thread-like adhesive body according to [1] or [2], wherein the twist coefficient of the core material is 25 to 120. [4] The thread-like adhesive body according to any one of [1] to [3], wherein the core material is a braided cord. [5] The thread-like adhesive body according to any one of [1] to [4], wherein the pressure-sensitive adhesive comprises a base polymer and a tackifier resin, and the pressure-sensitive adhesive comprises 1 to 100 parts by mass of the tackifier resin per 100 parts by mass of the base polymer. [6] The thread-like adhesive body according to any one of [1] to [5], wherein the pressure-sensitive adhesive is an acrylic pressure-sensitive adhesive.
[0103] The present invention will be explained in more detail below by way of examples, but the present invention is not limited to the following examples in any way.
[0104] <Preparation of Acrylic Polymer Emulsion> (Preparation of Acrylic Polymer Emulsion 1) 40 parts by mass of ion-exchanged water was placed in a reaction vessel equipped with a condenser, a nitrogen inlet tube, a thermometer, and a stirrer, and nitrogen substitution was carried out by stirring at 60°C for at least 1 hour while introducing nitrogen gas. 0.1 parts by mass of 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] n-hydrate (polymerization initiator) was added to this reaction vessel. While maintaining the reaction solution at 60°C, Monomer Emulsion A below was gradually added dropwise over 4 hours to allow the emulsion polymerization reaction to proceed.
[0105] Monomer emulsion A was prepared by adding 85 parts by mass of 2-ethylhexyl acrylate (2EHA), 13 parts by mass of methyl methacrylate (MA), 1.25 parts by mass of acrylic acid (AA), 0.75 parts by mass of methacrylic acid (MAA), 0.05 parts by mass of lauryl mercaptan (chain transfer agent), 0.02 parts by mass of γ-methacryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., trade name "KBM-503"), and 2 parts by mass of sodium polyoxyethylene lauryl sulfate (emulsifier) to 30 parts by mass of ion-exchanged water and emulsifying the mixture.
[0106] After the dropwise addition of Monomer Emulsion A was completed, the reaction liquid was further maintained at 60°C for 3 hours, cooled to room temperature, and then the pH was adjusted to 7 by adding 10% aqueous ammonia, thereby obtaining Acrylic Polymer Emulsion 1 (water-dispersed acrylic polymer).
[0107] (Preparation of Acrylic Polymer Emulsion 2) 40 parts by mass of ion-exchanged water was placed in a reaction vessel equipped with a cooling tube, a nitrogen inlet tube, a thermometer, and a stirrer, and nitrogen substitution was carried out by stirring at 60°C for at least 1 hour while introducing nitrogen gas. 0.1 parts by mass of 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] n-hydrate (polymerization initiator) was added to this reaction vessel. While maintaining the reaction liquid at 60°C, Monomer Emulsion B below was gradually added dropwise over 4 hours to allow the emulsion polymerization reaction to proceed.
[0108] Monomer emulsion B was prepared by adding 68 parts by mass of butyl acrylate (BA), 29.1 parts by mass of 2-ethylhexyl acrylate, 2.9 parts by mass of acrylic acid, 0.05 parts by mass of lauryl mercaptan (chain transfer agent), 0.03 parts by mass of γ-methacryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., trade name "KBM-503"), and 2 parts by mass of sodium polyoxyethylene lauryl sulfate (emulsifier) to 25 parts by mass of ion-exchanged water and emulsifying the mixture.
[0109] After the dropwise addition of Monomer Emulsion B was completed, the reaction liquid was further maintained at 60°C for 3 hours, cooled to room temperature, and then the pH was adjusted to 7 by adding 10% aqueous ammonia, thereby obtaining Acrylic Polymer Emulsion 2 (water-dispersed acrylic polymer).
[0110] (Preparation of Acrylic Polymer Emulsion 3) 40 parts by mass of ion-exchanged water was placed in a reaction vessel equipped with a cooling tube, a nitrogen inlet tube, a thermometer, and a stirrer, and nitrogen substitution was carried out by stirring at 60°C for at least 1 hour while introducing nitrogen gas. 0.1 parts by mass of 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] n-hydrate (polymerization initiator) was added to this reaction vessel. While maintaining the reaction liquid at 60°C, Monomer Emulsion C below was gradually added dropwise over 4 hours to allow the emulsion polymerization reaction to proceed.
[0111] Monomer emulsion C was prepared by adding 86.6 parts by mass of butyl acrylate, 9.6 parts by mass of 2-ethylhexyl acrylate, 3.8 parts by mass of acrylic acid, 0.055 parts by mass of lauryl mercaptan (chain transfer agent), 0.07 parts by mass of γ-methacryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., trade name "KBM-503"), and 2 parts by mass of sodium polyoxyethylene lauryl sulfate (emulsifier) to 29 parts by mass of ion-exchanged water and emulsifying the mixture.
[0112] After the dropwise addition of Monomer Emulsion C was completed, the reaction liquid was further maintained at 60°C for 3 hours, cooled to room temperature, and then the pH was adjusted to 7 by adding 10% aqueous ammonia, thereby obtaining Acrylic Polymer Emulsion 3 (water-dispersed acrylic polymer).
[0113] (Preparation of Acrylic Polymer Emulsion 4) 40 parts by mass of ion-exchanged water was placed in a reaction vessel equipped with a cooling tube, a nitrogen inlet tube, a thermometer, and a stirrer, and nitrogen substitution was carried out by stirring at 60°C for at least 1 hour while introducing nitrogen gas. 0.1 parts by mass of 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] n-hydrate (polymerization initiator) was added to this reaction vessel. While maintaining the reaction liquid at 60°C, Monomer Emulsion D was gradually added dropwise over 4 hours to allow the emulsion polymerization reaction to proceed.
[0114] Monomer emulsion D was prepared by adding 98 parts by mass of 2-ethylhexyl acrylate, 1.25 parts by mass of acrylic acid, 0.75 parts by mass of methacrylic acid, 0.05 parts by mass of lauryl mercaptan (chain transfer agent), 0.02 parts by mass of γ-methacryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., trade name "KBM-503"), and 2 parts by mass of sodium polyoxyethylene lauryl sulfate (emulsifier) to 30 parts by mass of ion-exchanged water and emulsifying the mixture.
[0115] After the dropwise addition of Monomer Emulsion D was completed, the reaction liquid was further maintained at 60°C for 3 hours, cooled to room temperature, and then the pH was adjusted to 7 by adding 10% aqueous ammonia, thereby obtaining Acrylic Polymer Emulsion 4 (water-dispersed acrylic polymer).
[0116] <Preparation of adhesive liquid (adhesive composition)>
[0117] (Preparation of Adhesive Liquid 1) A tackifier resin emulsion (manufactured by Arakawa Chemical Industries, Ltd., trade name "Tamanol E200NT") was added so that the tackifier resin was 35 parts by mass per 100 parts by mass of the acrylic polymer contained in the acrylic polymer emulsion 1. Further, ion-exchanged water was added to dilute the solid content to 45% by mass, and then 10% by mass ammonia water as a pH adjuster and polyacrylic acid (manufactured by Toagosei Co., Ltd., trade name "Aron B-500") as a thickener were used to adjust the pH and viscosity to be suitable for coating, thereby obtaining Adhesive Liquid 1.
[0118] (Preparation of Adhesive Liquid 2) A tackifier resin emulsion (manufactured by Arakawa Chemical Industries, Ltd., product name "Super Ester E865NT") was added so that the tackifier resin was 32 parts by mass per 100 parts by mass of the acrylic polymer contained in the acrylic polymer emulsion 1. Further, ion-exchanged water was added to dilute the solid content to 45% by mass, and then 10% by mass ammonia water as a pH adjuster and polyacrylic acid as a thickener were used to adjust the pH and viscosity to be suitable for coating, thereby obtaining Adhesive Liquid 2.
[0119] (Preparation of Adhesive Liquid 3) A tackifier resin emulsion (manufactured by Arakawa Chemical Industries, Ltd., product name "Tamanol E200NT") was added so that the tackifier resin was 35 parts by mass per 100 parts by mass of the acrylic polymer contained in the acrylic polymer emulsion 3. Further, ion-exchanged water was added to dilute the solid content to 45% by mass, and then 10% by mass of ammonia water as a pH adjuster and polyacrylic acid as a thickener were used to adjust the pH and viscosity to be suitable for coating, thereby obtaining Adhesive Liquid 3.
[0120] (Preparation of Adhesive Liquid 4) A tackifier resin emulsion (manufactured by Arakawa Chemical Industries, Ltd., product name "Tamanol E200NT") was added so that the tackifier resin was 35 parts by mass per 100 parts by mass of the acrylic polymer contained in the acrylic polymer emulsion 2. Further, ion-exchanged water was added to dilute the solid content to 45% by mass, and then 10% by mass of ammonia water as a pH adjuster and polyacrylic acid as a thickener were used to adjust the pH and viscosity to be suitable for coating, thereby obtaining Adhesive Liquid 4.
[0121] (Preparation of Adhesive Liquid 5) Adhesive liquid 5 was obtained in the same manner as Adhesive Liquid 1, except that the amount of the tackifier resin emulsion added was changed to 32 parts by mass of the tackifier resin per 100 parts by mass of the acrylic polymer.
[0122] (Preparation of Adhesive Liquid 6) A tackifier resin emulsion (manufactured by Arakawa Chemical Industries, Ltd., product name "Super Ester E865NT") was added so that the tackifier resin was 20 parts by mass per 100 parts by mass of the acrylic polymer contained in the acrylic polymer emulsion 4. Further, ion-exchanged water was added to dilute the solid content to 45% by mass, and then 10% by mass ammonia water as a pH adjuster and polyacrylic acid as a thickener were used to adjust the pH and viscosity to be suitable for coating, thereby obtaining Adhesive Liquid 6.
[0123] <Production of Thread-Like Adhesive> (Example 1) As a core material, a multifilament yarn was prepared by twisting 150 times per meter seven polyethylene terephthalate (PET) fibers (manufactured by Teijin Frontier Co., Ltd.) (fineness: 1169 dtex, number of filaments: 336) with a fineness of 167 dtex and a number of filaments: 48. The viscosity of adhesive liquid 1 was adjusted, and the core material was coated by dipping using a coating roller. The solution was then dried at 100°C for 1 minute to obtain a thread-like adhesive body with a glue amount (adhesive amount) of 40.0 mg / m.
[0124] Examples 2 to 6 Thread-like adhesive bodies were produced in the same manner as in Example 1, except that the twist number of the multifilament yarn was changed to 70, 90, 110, 200, and 300 times per meter, respectively. The amounts of adhesive were 73.8 mg / m, 42.2 mg / m, 41.5 mg / m, 36.7 mg / m, and 38.3 mg / m, respectively.
[0125] (Examples 7, 8, and 9) Thread-like adhesive bodies were prepared in the same manner as in Example 3, except that adhesive liquids 3, 4, and 2 were used instead of adhesive liquid 1. The amounts of adhesive were 33.8 mg / m, 39.8 mg / m, and 49.0 mg / m, respectively.
[0126] Example 10: A multifilament yarn was prepared as a core material, which was a hollow string made of 16 untwisted PET fibers (fineness: 62 dtex). The viscosity of adhesive liquid 5 was adjusted, and the core material was coated with the adhesive liquid by dipping using a coating roller. The resultant was then dried at 100°C for 1 minute, yielding a filament-like adhesive body with an adhesive amount of 43.3 mg / m.
[0127] Comparative Example 1 A thread-like adhesive body was produced in the same manner as in Example 1, except that the number of twists of the multifilament yarn was changed to 70 times per meter. The amount of adhesive was 51.0 mg / m.
[0128] Comparative Example 2 A thread-like adhesive body was produced in the same manner as in Example 1, except that adhesive liquid 6 was used instead of adhesive liquid 1 and the twist number of the multifilament yarn was changed to 350 times per meter. The amount of adhesive was 130.0 mg / m.
[0129] Comparative Example 3 A thread-like adhesive body was produced in the same manner as in Example 1, except that the number of twists of the multifilament yarn was changed to 30 times per meter. The amount of adhesive was 137.0 mg / m.
[0130] <Properties of thread-like adhesive body> (Amount of adhesive and amount of adhesive attached to core material) The amount of adhesive was calculated using the mass per unit length of the core material W1 [mg / m] and the mass per unit length of the thread-like adhesive body after coating and drying with the adhesive W2 [mg / m], according to the following formula (2). Adhesive amount [mg / m] = W2 [mg / m] - W1 [mg / m] (2) The amount of adhesive attached to the core material was calculated using the following formula (3). Amount of adhesive attached to core material [mass %] = {(W2 - W1) / W1} × 100 (3)
[0131] (Width-direction length and width-direction length variation of thread-like adhesive body) The thread-like adhesive bodies of the Examples and Comparative Examples were observed under a microscope, and the width-direction length (length perpendicular to the longitudinal direction) of the thread-like adhesive body was measured at 10 points at 1 cm intervals in the longitudinal direction, and the average value m and standard deviation (3σ) were calculated. Specifically, the thread-like adhesive body was first placed on the stage of the microscope, and its position was finely adjusted so that the latitude lines of the grid-like scale displayed on the observation screen were parallel to the long axis of the thread-like adhesive body. The observation magnification of the microscope was set to 30x, and the length of the short axis (width-direction length) of the thread-like adhesive body was measured at 10 points at 1 cm intervals in the longitudinal direction. The maximum value at each measurement point was used as the width-direction length of the thread-like adhesive body. The obtained measurement value (X 1 , X 2 ,...,X 10 ) was used to calculate the average value m, which was taken as the average length of the thread-like adhesive bodies in the width direction. In addition, the standard deviation 3σ (μm) was calculated using the following formula (4).
[0132]
[0133] In formula (4), X 1 , X 2 ,...,X n represents each measured value, m represents the average value, and n represents the number of data. In the above measurement method, n is 10.
[0134] <Evaluation> The obtained thread-like adhesive bodies were evaluated as follows. The results are shown in Tables 1 to 3.
[0135] (Adhesive Strength) The adhesive strength of the thread-like adhesive body was evaluated using the cleavage peel force described below. Figures 3 to 5 are diagrams illustrating a method for evaluating the adhesive strength of a thread-like adhesive body according to an embodiment of the present invention. The obtained thread-like adhesive body 40 was arranged on a stainless steel (SUS) plate 3a (W (mm) x D (mm) x H (mm) = 30 x 60 x 2) in a spiral shape with an outer diameter of 25 mm, 5 circumferences, a pitch distance of 1.5 mm, and a usage length of 27 cm, as shown in Figure 3. On top of this, a SUS plate 3b (W (mm) x D (mm) x H (mm) = 30 x 30 x 3) was placed as shown in Figure 4, and the resulting mixture was pressed with a press under a pressure of 0.35 MPa for 10 seconds to obtain a bonded body 20 for evaluation. The obtained bonded body 20 for evaluation was set in a tensile tester (Shimadzu Autograph AG-100M2 manufactured by Shimadzu Corporation), and peeled in a direction perpendicular to the plane of the plate 3b as shown in FIG. 5 under conditions of 23°C and a tensile speed of 300 mm / min, and the obtained stress value was defined as the adhesive strength (MPa).
[0136] (Waterproofing) Using the thread-like adhesive of each example, a polycarbonate (PC) resin plate (3 cm on each side) and a slightly larger PC resin plate (4 cm on each side, square) were bonded to prepare a test specimen. Specifically, as shown in FIG. 6, a thread-like adhesive 1 was first placed on one polycarbonate resin plate 4a in a square shape with a side length X of 2.5 cm and an overlap Y of 1 cm at the tip of the thread-like adhesive. A nonwoven fabric 5 (1.5 cm square) was then placed inside the square, and the other PC resin plate 4b was then laminated on top of it as shown in FIG. 7. The resulting test specimen was then pressed with a press under a pressure of 0.35 MPa for 10 seconds to obtain a bonded assembly for evaluation. The resulting test specimen was then placed in a water bath, held at a depth of 1 m for 30 minutes, and then removed. If water did not penetrate into the area surrounded by the thread-like adhesive bodies of the removed test piece, it was evaluated as ◯, and if water penetrated, it was evaluated as ×.
[0137] In the following Tables 1 to 3, the polymer column shows the type of monomer and the amount (parts by mass) of each monomer constituting the polymer.
[0138]
[0139]
[0140]
[0141] The results shown in Tables 1 to 3 demonstrate that the thread-like adhesive bodies of Examples 1 to 10, in which the standard deviation 3σ of the widthwise length of the thread-like adhesive bodies was 100 μm or less, were excellent in waterproofing. They also had sufficient adhesive strength as thread-like adhesive bodies. In contrast, the thread-like adhesive bodies of Comparative Examples 1 to 3, in which 3σ exceeded 100 μm, did not achieve the desired waterproofing.
[0142] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention.
[0143] By using the thread-like adhesive material of the present invention, it is possible to provide a thread-like adhesive material having excellent waterproof properties.
[0144] Although the present invention has been described in detail and with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on a Japanese patent application (Patent Application No. 2023-58693) filed on March 31, 2023, the contents of which are incorporated herein by reference.
[0145] 40 Thread-like adhesive body 2a, 2b Housing 3a, 3b Board 4a, 4b Resin board 5 Nonwoven fabric 10 Joined body
Claims
1. A filamentous adhesive comprising a core material and an adhesive coating the longitudinal surface of the core material, wherein the standard deviation 3σ of the widthwise length of the filamentous adhesive calculated by the following method is 100 μm or less, and the core material is a multifilament yarn comprising 4 or more filaments. (Calculation method) The average widthwise length and standard deviation 3σ of the widthwise length of the filamentous adhesive are calculated by observing the filamentous adhesive with a microscope, measuring the widthwise length at 10 points at intervals of 1 cm in the longitudinal direction, and calculating the average value and standard deviation 3σ of those values. The widthwise length of the filamentous adhesive is the maximum value at each measurement point.
2. The thread-like adhesive body according to claim 1, wherein the amount of the adhesive attached is 20 to 80% by mass relative to the core material.
3. A thread-like adhesive body according to claim 1 or 2, wherein the twist factor of the core material is 25 to 120.
4. The thread-like adhesive body according to claim 1 or 2, wherein the core material is a braided cord.
5. A thread-like adhesive body as described in claim 1 or 2, wherein the adhesive comprises a base polymer and a tackifier resin, and the adhesive contains 1 to 100 parts by mass of the tackifier resin per 100 parts by mass of the base polymer.
6. The thread-like adhesive body according to claim 1 or 2, wherein the adhesive is an acrylic adhesive.
Citation Information
Patent Citations
Adhesive article
JP2020076066A
gaming machines
JP2023058693A
Filamentous adhesive body and filamentous adhesive body manufacturing method
JP2021055091A
Filamentous adhesive body and filamentous adhesive body manufacturing method
JP2021055252A
Device and method for applying filamentous adhesive
JP2021161407A
Cited By
Threadlike adhesive body
WO2025143264A1