Electrically removable pressure-sensitive adhesive sheet and bonded object
The electrically peelable adhesive sheet with a resin-containing conductive base and ionic liquid adhesive layer addresses peeling issues in high-temperature, high-humidity environments by maintaining adhesive strength and facilitating easy peeling, enhancing reliability and connectivity.
Patent Information
- Application Number
- PCT/JP2024/012277
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-01-31
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional electrically peelable adhesive sheets fail to maintain adhesive strength and reliability when exposed to high-temperature, high-humidity environments, leading to peeling issues and contamination due to corrosion of the conductive layer.
An electrically peelable adhesive sheet with a conductive base material containing a resin component and an adhesive layer that decreases adhesive strength when voltage is applied, ensuring contact between the conductive layer and the adhesive layer, using ionic liquids and conductive polymers like PEDOT/PSS, and optionally including conductive fillers to prevent peeling and maintain adhesion.
The solution effectively suppresses peeling of the conductive layer from the substrate and maintains sufficient adhesive strength even in harsh environments, ensuring reliable electrical connectivity and easy peeling when required.
Smart Images

Figure JP2024012277_03102024_PF_FP_ABST
Abstract
Description
Electrically peelable adhesive sheet and bonded body
[0001] The present invention relates to an electrically releasable pressure-sensitive adhesive sheet and a bonded body.
[0002] In electronic component manufacturing processes, etc., there is an increasing demand for rework to improve yields and recycling by disassembling and recovering components after use. To meet these demands, double-sided electrically peelable pressure-sensitive adhesive sheets that have a certain level of adhesive strength and releasability are sometimes used to join components in electronic component manufacturing processes, etc.
[0003] A known double-sided electrically peelable adhesive sheet that achieves the above-mentioned adhesive strength and releasability is an electrically peelable adhesive sheet (electrically peelable adhesive sheet) that uses an ionic liquid consisting of cations and anions as the component that forms the adhesive layer, and whose adhesive strength is reduced by applying a voltage to the adhesive layer, thereby making it easy to peel off.
[0004] For example, Patent Document 1 describes an electrically releasing pressure-sensitive adhesive sheet that uses a conductive substrate having a metal vapor deposition layer on a support substrate as the conductive substrate, and that includes, in this order, a support substrate, a conductive layer (metal layer), a coating layer for protecting the conductive layer, and an electrically releasing pressure-sensitive adhesive layer whose adhesive strength decreases upon application of a voltage. Patent Document 1 describes a method in which, when the electrically releasing pressure-sensitive adhesive layer of the electrically releasing pressure-sensitive adhesive sheet is attached to a conductive support, a voltage is applied between the conductive support attached using the pressure-sensitive adhesive layer and the conductive substrate, thereby peeling the electrically releasing pressure-sensitive adhesive sheet from the conductive support.
[0005] Japanese Patent Application Publication No. 2022-126243
[0006] It is preferable that the electrically peelable pressure-sensitive adhesive sheet firmly bonds members when no voltage is applied, and can be peeled off with little force when a voltage is applied.
[0007] However, in the conventional technology described in Patent Document 1, when an assembly in which an electrically-release pressure-sensitive adhesive sheet is attached to a conductive adherend is placed in a high-temperature, high-humidity environment for a long period of time (e.g., 600 hours or more), the coating layer protecting the conductive layer deteriorates and the conductive layer (metal layer) corrodes, causing the conductive layer to peel off from the support substrate when electrical peeling is attempted, resulting in the electrically-release pressure-sensitive adhesive sheet not functioning properly. This is thought to be because the conductive substrate is not electrically connected to the electrically-release pressure-sensitive adhesive layer, making it impossible to apply voltage to the electrically-release pressure-sensitive adhesive layer via the conductive substrate and the conductive adherend. As a result, for example, the adhesive strength of the electrically-release pressure-sensitive adhesive layer does not decrease sufficiently, making it difficult to peel or leaving adhesive residue. Furthermore, there is a risk that the conductive layer will peel off from the support substrate when electrical peeling is attempted, leading to contamination of the adherend. The present invention was completed in view of the above, and a first object of the present invention is to provide an electrically-release pressure-sensitive adhesive sheet and assembly that can suppress peeling of the conductive layer from the support substrate even when placed in a high-temperature, high-humidity environment for a long period of time.
[0008]
[0006] Furthermore, in the conventional technology described in Patent Document 1, when an assembly in which an electrically releasing pressure-sensitive adhesive sheet is attached to a conductive adherend is placed in a high-temperature, high-humidity environment for a long period of time, the adhesive strength between the electrically releasing pressure-sensitive adhesive layer constituting the electrically releasing pressure-sensitive adhesive sheet and the conductive substrate may decrease due to deterioration of the coating layer protecting the conductive layer, resulting in peeling. As a result, an assembly formed using an electrically releasing pressure-sensitive adhesive sheet may not be able to achieve reliable adhesion. The present invention has been completed in view of the above, and a second object of the present invention is to provide an electrically releasing pressure-sensitive adhesive sheet and an assembly that can prevent a decrease in the adhesive strength between the electrically releasing pressure-sensitive adhesive layer constituting the electrically releasing pressure-sensitive adhesive sheet and the conductive substrate even when placed in a high-temperature, high-humidity environment for a long period of time, thereby suppressing a decrease in the adhesive strength of the electrically releasing pressure-sensitive adhesive sheet.
[0009] As a result of extensive investigations, the present inventors have found that by providing an electrically releasing pressure-sensitive adhesive sheet comprising, in this order, a conductive substrate including a support substrate and a conductive layer containing a resin component, and an electrically releasing pressure-sensitive adhesive layer, in which the electrically releasing pressure-sensitive adhesive layer and the conductive layer are in contact with each other, peeling of the conductive layer from the support substrate can be suppressed even when stored under high temperature and high humidity conditions for a long period of time. They have also found that peeling of the electrically releasing pressure-sensitive adhesive layer and the conductive layer can be suppressed.
[0010] The means for solving the above problems are as follows. [1] An electrically releasing pressure-sensitive adhesive sheet comprising: a conductive substrate including a support substrate and a conductive layer containing a resin component; and an electrically releasing pressure-sensitive adhesive layer whose adhesive strength decreases upon application of a voltage, the electrically releasing pressure-sensitive adhesive layer being in contact with the conductive layer. [2] The electrically releasing pressure-sensitive adhesive sheet according to [1], wherein the electrically releasing pressure-sensitive adhesive layer contains a polymer and an ionic liquid. [3] The electrically releasing pressure-sensitive adhesive sheet according to [2], wherein the anion of the ionic liquid is at least one selected from the group consisting of bis(fluorosulfonyl)imide anion and bis(trifluoromethanesulfonyl)imide anion. [4] The electrically releasing pressure-sensitive adhesive sheet according to [2], wherein the cation of the ionic liquid is at least one selected from the group consisting of nitrogen-containing onium cations, sulfur-containing onium cations, and phosphorus-containing onium cations. [5] The electrically releasing pressure-sensitive adhesive sheet according to [1] or [2], wherein the conductive layer contains a conductive polymer. [6] The electrically peelable pressure-sensitive adhesive sheet according to [5], wherein the conductive polymer comprises at least one selected from PEDOT / PSS, a polyacetylene-based polymer, a polyaniline-based polymer, and a polypyrrole-based polymer. [7] The electrically peelable pressure-sensitive adhesive sheet according to [1] or [2], wherein the conductive layer further comprises a conductive filler. [8] The electrically peelable pressure-sensitive adhesive sheet according to [7], wherein the conductive filler is carbon particles or metal particles. [9] The electrically peelable pressure-sensitive adhesive sheet according to [1] or [2], wherein the conductive layer has a surface resistance of 5000 Ω / □ or less.
[10] The electrically peelable pressure-sensitive adhesive sheet according to [1] or [2], further comprising another pressure-sensitive adhesive layer, the other pressure-sensitive adhesive layer being formed on the surface of the support substrate opposite to the conductive layer.
[11] The electrically peeling pressure-sensitive adhesive sheet according to [1] or [2], further comprising another pressure-sensitive adhesive layer, a second conductive layer containing a resin component, and a second other pressure-sensitive adhesive layer, wherein the other pressure-sensitive adhesive layer is formed on the surface of the support substrate opposite to the conductive layer, and the second conductive layer and the second other pressure-sensitive adhesive layer are formed in this order on the surface of the electrically peeling pressure-sensitive adhesive layer opposite to the conductive layer, and the electrically peeling pressure-sensitive adhesive layer and the second conductive layer are in contact with each other.
[12] A joined body comprising the electrically peeling pressure-sensitive adhesive sheet according to [1] or [2] and a conductive material, wherein the electrically peeling pressure-sensitive adhesive layer is adhered to the conductive material.
[13] A joined body comprising the electrically peeling pressure-sensitive adhesive sheet according to
[11] and an adherend material, wherein the other pressure-sensitive adhesive layer is adhered to the adherend material.
[0011] The electrically peelable pressure-sensitive adhesive sheet of the present invention can suppress peeling of the conductive layer from the support substrate due to application of voltage, and can suppress peeling of the electrically peelable pressure-sensitive adhesive layer from the conductive layer, even when stored in a high-temperature, high-humidity environment for a long period of time, thereby maintaining sufficient adhesive strength.
[0012] Fig. 1 is a schematic cross-sectional view showing one example of the electrically peelable pressure-sensitive adhesive sheet of the present invention. Fig. 2 is a schematic cross-sectional view showing another example of the electrically peelable pressure-sensitive adhesive sheet of the present invention. Fig. 3 is a cross-sectional view showing an outline of a method for a 180° peel test in the examples.
[0013] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The following describes in detail the preferred embodiments of the present invention, but the present invention is not limited to the following preferred embodiments.
[0014] [Electrically Peelable Pressure-Sensitive Adhesive Sheet] [Configuration of Electrically Peelable Pressure-Sensitive Adhesive Sheet] The electrically peelable pressure-sensitive adhesive sheet according to an embodiment of the present invention comprises a conductive substrate including a support substrate and a conductive layer containing a resin component, and an electrically peelable pressure-sensitive adhesive layer whose adhesive strength decreases upon application of a voltage, and the electrically peelable pressure-sensitive adhesive layer and the conductive layer are in contact with each other.
[0015] The inventors of the present invention believe that the reason why the electrically releasing pressure-sensitive adhesive sheet according to the embodiment of the present invention is able to suppress peeling of the conductive layer from the support substrate due to application of voltage, suppress peeling of the electrically releasing pressure-sensitive adhesive layer from the conductive layer, and maintain sufficient adhesive strength when no voltage is applied, even when stored in a high-temperature, high-humidity environment for a long period of time, and is able to function as an electrically releasing pressure-sensitive adhesive sheet, is as follows: Here, "the electrically releasing pressure-sensitive adhesive sheet according to the embodiment of the present invention functions" means that a voltage can be applied to the electrically releasing pressure-sensitive adhesive layer via the conductive substrate, thereby reducing the adhesive strength of the electrically releasing pressure-sensitive adhesive layer and allowing it to be easily peeled.
[0016] In conventional electrically peelable pressure-sensitive adhesive sheets, a metal layer is used as the conductive layer, and a coating layer is provided to protect the conductive layer (metal layer). However, when exposed to high temperature and humidity for a long period of time, the resin components in the coating layer hydrolyze, causing the coating layer to deteriorate, exposing the conductive layer and corroding the metal. Therefore, when voltage is applied, the conductive layer may peel off from the support substrate, causing the sheet to no longer function as an electrically peelable pressure-sensitive adhesive sheet. In addition, the deterioration of the coating layer may reduce the adhesive strength between the electrically peelable pressure-sensitive adhesive layer and the conductive substrate, resulting in peeling.
[0017] On the other hand, the conductive substrate in the electrically peelable pressure-sensitive adhesive sheet according to an embodiment of the present invention comprises a support substrate and a conductive layer containing a resin component. Although the details of the mechanism are unclear, the use of a conductive layer containing a resin component makes the conductive layer less susceptible to corrosion even when exposed to high temperature and high humidity for a long period of time, thereby preventing the conductive layer from peeling off from the support substrate when a voltage is applied. Furthermore, the inclusion of a resin component in the conductive layer improves the adhesion between the electrically peelable pressure-sensitive adhesive layer and the conductive substrate, thereby preventing peeling within the electrically peelable pressure-sensitive adhesive sheet exposed to high temperature and high humidity for a long period of time. Furthermore, the electrically peelable pressure-sensitive adhesive sheet according to an embodiment of the present invention does not require a coating layer for protecting the conductive layer, thereby preventing a decrease in electrical peeling performance due to deterioration of the coating layer and a decrease in the adhesive strength between the electrically peelable pressure-sensitive adhesive layer and the conductive substrate. From this perspective, in the electrically peelable pressure-sensitive adhesive sheet according to an embodiment of the present invention, the conductive layer is preferably provided by a means other than metal vapor deposition, and preferably does not include a metal layer.
[0018] The electrically releasing pressure-sensitive adhesive sheet according to the embodiment of the present invention may have a plurality of conductive substrates and a plurality of electrically releasing pressure-sensitive adhesive layers, or may have a pressure-sensitive adhesive layer, an intermediate layer, an undercoat layer, etc. in addition to the conductive substrate and the electrically releasing pressure-sensitive adhesive layer. Furthermore, in the electrically releasing pressure-sensitive adhesive sheet according to the embodiment of the present invention, the conductive substrate may have a plurality of support substrates and a plurality of conductive layers containing a resin component. The electrically releasing pressure-sensitive adhesive sheet according to the embodiment of the present invention may be, for example, in the form of a roll or in the form of a sheet. The term "electrically releasing pressure-sensitive adhesive sheet" also includes the meaning of "adhesive tape." That is, the electrically releasing pressure-sensitive adhesive sheet according to the embodiment of the present invention may be an adhesive tape in the form of a tape.
[0019] The electrically releasing pressure-sensitive adhesive sheet according to an embodiment of the present invention may be a single-sided electrically releasing pressure-sensitive adhesive sheet having a conductive substrate and an electrically releasing pressure-sensitive adhesive layer on only one side of the conductive substrate. The electrically releasing pressure-sensitive adhesive sheet according to an embodiment of the present invention may further comprise another pressure-sensitive adhesive layer that does not have electrical release properties, or may further comprise another pressure-sensitive adhesive layer on the surface of the electrically releasing pressure-sensitive adhesive sheet facing the support substrate. The electrically releasing pressure-sensitive adhesive sheet according to an embodiment of the present invention may also be a double-sided electrically releasing pressure-sensitive adhesive sheet having a conductive substrate having conductive layers on both sides of the support substrate, and an electrically releasing pressure-sensitive adhesive layer on each conductive layer. The electrically releasing pressure-sensitive adhesive sheet according to an embodiment of the present invention may have a release liner for the purpose of protecting the electrically releasing pressure-sensitive adhesive layer and the surface of the other pressure-sensitive adhesive layers, but such release liner is not included in the electrically releasing pressure-sensitive adhesive sheet according to an embodiment of the present invention.
[0020] The electrically peelable pressure-sensitive adhesive sheet according to the embodiment of the present invention is also preferably an electrically peelable pressure-sensitive adhesive sheet further comprising another pressure-sensitive adhesive layer, the other pressure-sensitive adhesive layer being formed on the surface of the supporting substrate opposite to the conductive layer.
[0021] Furthermore, the electrically peeling pressure-sensitive adhesive sheet according to an embodiment of the present invention is also preferably an electrically peeling pressure-sensitive adhesive sheet further comprising another pressure-sensitive adhesive layer, a second conductive layer containing a resin component, and a second other pressure-sensitive adhesive layer, wherein the other pressure-sensitive adhesive layer is formed on the surface of the support substrate opposite to the conductive layer, and the second conductive layer and the second other pressure-sensitive adhesive layer are formed in this order on the surface of the electrically peeling pressure-sensitive adhesive layer opposite to the conductive layer, and the electrically peeling pressure-sensitive adhesive layer and the second conductive layer are in contact with each other.
[0022] The structure of the electrically peelable adhesive sheet according to the embodiment of the present invention is not particularly limited, but preferred examples include electrically peelable adhesive sheet X1 shown in FIG. 1, electrically peelable adhesive sheet X2 shown in FIG. 2, and electrically peelable adhesive sheet X3 shown in FIG. 3.
[0023] The electrically peelable pressure-sensitive adhesive sheet X1 shown in FIG. 1 is an electrically peelable pressure-sensitive adhesive sheet having a layer structure of an electrically peelable pressure-sensitive adhesive layer 1 and a conductive substrate 5 (conductive layer 3 and supporting substrate 4).
[0024] The electrically peelable pressure-sensitive adhesive sheet X2 shown in Figure 2 is an electrically peelable pressure-sensitive adhesive sheet having a layer structure of another pressure-sensitive adhesive layer 6, a conductive substrate 5 (support substrate 4 and conductive layer 3), and an electrically peelable pressure-sensitive adhesive layer 1.
[0025] The electrically releasing pressure-sensitive adhesive sheet X3 shown in Fig. 3 is an electrically releasing pressure-sensitive adhesive sheet having a layer configuration comprising, in this order, another pressure-sensitive adhesive layer 6, a conductive substrate 5 (supporting substrate 4, conductive layer 3), an electrically releasing pressure-sensitive adhesive layer 1, a conductive substrate 5 (conductive layer 3, supporting substrate 4), and another pressure-sensitive adhesive layer 6. That is, the electrically releasing pressure-sensitive adhesive layer 1 in the electrically releasing pressure-sensitive adhesive sheet X3 shown in Fig. 3 is a double-sided electrically releasing pressure-sensitive adhesive sheet comprising, on both sides thereof, a conductive layer 3, a supporting substrate 4, and another pressure-sensitive adhesive layer 6, in this order.
[0026] The conductive layer 3 containing a resin component is formed on a supporting substrate 4 and is a layer in contact with the electrically peelable pressure-sensitive adhesive layer 1 .
[0027] Because the conductive layer 3 contains a resin component, the conductive layer is less likely to corrode even when exposed to high temperature and humidity for a long period of time, and also acts as a barrier to the ionic liquid contained in the electrically peelable pressure-sensitive adhesive layer 1 from penetrating into the conductive layer 3 when a voltage is applied, thereby preventing the conductive layer 3 from peeling off from the support substrate 4.
[0028] Furthermore, since the conductive layer 3 containing a resin component is in contact with the electrically peeling adhesive layer 1, the adhesion between the electrically peeling adhesive layer 1 and the conductive layer 3 is improved, and this has the effect of preventing the interfacial adhesion between the electrically peeling adhesive layer and the conductive layer from decreasing due to thermal hardening of the electrically peeling adhesive layer when exposed to a high temperature and high humidity environment for a long period of time, thereby preventing peeling within the electrically peeling adhesive sheet.
[0029] Examples of resin components contained in the conductive layer 3 according to the embodiment of the present invention include conductive polymers, non-conductive polymers, conductive oligomers, thermoplastic resins, and thermosetting resins. Because the electrically releasing pressure-sensitive adhesive sheet is released by applying a voltage to the electrically releasing pressure-sensitive adhesive layer, it is preferable that the conductive layer contain a conductive polymer from the viewpoint of electrical connection. Examples of conductive polymers according to the embodiment of the present invention include PEDOT / PSS (a composite of poly(3,4-ethylenedioxythiophene) (PEDOT) and polystyrene sulfonic acid (PSS)), polyacetylene-based polymers, polyaniline-based polymers, and polypyrrole-based polymers. Of these, PEDOT / PSS is preferred as the conductive polymer from the viewpoint of ease of availability. The conductive polymers can be used alone or in combination of two or more. That is, it is preferable that the conductive polymer contain at least one selected from PEDOT / PSS, polyacetylene-based polymers, polyaniline-based polymers, and polypyrrole-based polymers.
[0030] When the resin component is a conductive polymer, the content of the resin component in the conductive layer is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, relative to the total amount (100% by mass) of the conductive layer, and the upper limit may be 100% by mass or less, or may be 99.9% by mass or less, or may be 99.5% by mass or less.
[0031] The conductive layer 3 according to the embodiment of the present invention may further contain various additives such as a crosslinking agent, a catalyst, a filler, a plasticizer, an antioxidant, an antioxidant, a pigment (dye), a flame retardant, a solvent, a surfactant (leveling agent), a dispersant, a rust inhibitor, and a corrosion inhibitor. The total content of these components is not particularly limited as long as the effects of the present invention are achieved, but is preferably 0.01 parts by mass or more and 20 parts by mass or less, more preferably 10 parts by mass or less, and even more preferably 5 parts by mass or less, per 100 parts by mass of the resin component. The conductive layer 3 according to the embodiment of the present invention may further contain a conductive filler, which will be described later.
[0032] The resin component contained in the conductive layer 3 according to the embodiment of the present invention may be a non-conductive polymer. When the resin component is a non-conductive polymer, the conductive layer preferably contains a conductive filler or the like for the purpose of imparting conductivity. The conductive layer 3 according to the embodiment of the present invention may be formed from a conductive paste containing a resin component and a conductive filler.
[0033] Examples of the non-conductive polymer according to the embodiment of the present invention include acrylic resins, polyester resins, epoxy resins, urethane resins, phenolic resins, and epoxy resins. At least one resin selected from acrylic resins, urethane resins, epoxy resins, and polyester resins is preferred, and at least one resin selected from acrylic resins, urethane resins, and epoxy resins is more preferred.
[0034] Examples of acrylic resins include poly(meth)acrylic acid esters such as polymethyl methacrylate, methyl methacrylate-(meth)acrylic acid copolymers, methyl methacrylate-(meth)acrylic acid ester copolymers, methyl methacrylate-acrylic acid ester-(meth)acrylic acid copolymers, methyl (meth)acrylate-styrene copolymers (MS resins, etc.), and polymers having an alicyclic hydrocarbon group (for example, methyl methacrylate-cyclohexyl methacrylate copolymers, methyl methacrylate-norbornyl (meth)acrylate copolymers, etc.).
[0035] In this specification, "(meth)acrylic" means acrylic and / or methacrylic. Acrylic resins include those containing acrylic acid or a derivative thereof as a constituent monomer component, and those containing methacrylic acid or a derivative thereof as a constituent monomer component.
[0036] Examples of urethane-based resins include oil-modified polyurethane resins, alkyd-based polyurethane resins, polyester-based polyurethane resins, and polyether-based urethane resins, with polyether-based urethane resins being preferred from the viewpoint of inhibiting hydrolysis.
[0037] Examples of epoxy resins include crosslinked resins obtained by crosslinking epoxy groups present in epoxy group-containing monomers or epoxy group-containing prepolymers with a curing agent (such as a photopolymerization initiator or a thermal polymerization initiator).Specific examples of epoxy resins include bisphenol A epoxy resins, bisphenol F epoxy resins, cresol novolac epoxy resins, alicyclic epoxy resins, and phenol novolac epoxy resins.
[0038] The non-conductive polymer may be crosslinkable. The non-conductive polymer may be used alone or in combination of two or more kinds.
[0039] When the resin component according to the embodiment of the present invention is a non-conductive polymer, the content of the resin component in the conductive layer is preferably 0.1% by mass or more, more preferably 1.0% by mass or more, relative to the total amount (100% by mass) of the conductive layer, and the upper limit is preferably 70% by mass or less, more preferably 30% by mass or less.
[0040] The conductive filler contained in the conductive layer according to the embodiment of the present invention is not particularly limited, and a commonly known or commonly used conductive filler can be used, such as particles made of metal, metal oxide, carbon, conductive polymer, metal-coated particles, etc. Among these, carbon particles or metal particles are preferably used because of their ease of handling. These can be used alone or in combination of two or more types.
[0041] The shape of the conductive filler according to the embodiment of the present invention is not particularly limited, but examples thereof include spherical, rod-like, plate-like, fibrous, hollow, angular, lumpy, and aggregates thereof. Among these, it is preferable to use primary aggregates of spherical particles, since this makes it easy to control the proportion of conductive filler contained in the conductive layer.
[0042] The average particle size of the conductive filler according to the embodiment of the present invention is preferably 0.001 μm or more, more preferably 0.05 μm or more, even more preferably 0.1 μm or more, even more preferably 0.2 μm or more, and particularly preferably 0.5 μm or more. The average particle size is preferably 30 μm or less, more preferably 20 μm or less, more preferably 10 μm or less, and even more preferably 5 μm or less. The average particle size of the conductive filler is preferably 0.001 to 30 μm, and more preferably 0.001 to 20 μm. Having the average particle size within the above range is preferable in terms of maintaining the viscosity of the conductive paste and the dispersibility of the conductive filler. Furthermore, when the conductive filler is carbon particles, the average particle size is preferably 0.001 to 30 μm, more preferably 0.001 to 20 μm, and even more preferably 0.05 to 10 μm. When the particle size of the carbon particles is 0.001 μm or more, the increase in the amount of added carbon particles is suppressed, and the increase in viscosity of the conductive paste is suppressed, resulting in excellent coatability. Furthermore, when the particle size of the carbon particles is 30 μm or less, conductive paths are easily formed, and sufficient conductivity is easily obtained. When the conductive filler is silver particles, the average particle size is preferably 0.1 to 30 μm, more preferably 0.1 to 10 μm, and even more preferably 0.2 to 5 μm. When the particle size of the silver particles is 0.1 μm or more, the increase in the amount of added silver particles is suppressed, and the increase in viscosity of the conductive paste is suppressed, resulting in excellent coatability. Furthermore, when the particle size of the silver particles is 30 μm or less, conductive paths are easily formed, and sufficient conductivity is easily obtained. Note that, in this specification, the average particle size of the conductive filler refers to the particle size at which the cumulative particle size on a weight basis is 50% (50% median diameter) in the particle size distribution obtained by measurement based on the sieving method.
[0043] Examples of the carbon particles include graphite, carbon black, acetylene black, ketjen black, carbon nanofibers, carbon nanotubes, graphene, fullerenes, carbon nanocoils, carbon microcoils, carbon beads, and carbon fibers. Of these, carbon black is preferably used because of its low cost and easy availability.
[0044] The carbon black is not particularly limited, but may be, for example, one having a particle diameter of 50 nm or less and a specific surface area of 50 m 2 / 100g or more, DBP adsorption capacity 100cm 3 / 100g or more is preferably used.
[0045] Examples of the metal include particles of silver, copper, aluminum, nickel, iron, gold, stainless steel, and alloys thereof, and from the viewpoint of electrical conductivity, silver, gold, copper, and aluminum are preferred, with silver being more preferred. Examples of the metal oxide include particles of zinc oxide, indium oxide, tin oxide, titanium oxide, and zirconium oxide.
[0046] When the conductive layer according to the embodiment of the present invention contains a conductive filler, the content of the conductive filler is preferably 0.1 parts by mass or more and 9,900 parts by mass or less relative to 100 parts by mass of the non-conductive polymer. The lower limit of the conductive filler content is preferably 3 parts by mass or more, more preferably 5 parts by mass or more, more preferably 10 parts by mass or more, more preferably 100 parts by mass or more, more preferably 200 parts by mass or more, more preferably 300 parts by mass or more, and even more preferably 400 parts by mass or more. The upper limit may be 4,000 parts by mass or less, 2,000 parts by mass or less, or even 1,000 parts by mass or less. A content of the conductive filler within the above range is preferable in terms of maintaining good viscosity of the conductive paste and good dispersibility of the conductive filler. Furthermore, when the conductive filler is carbon particles, the lower limit of the carbon particle content is preferably 0.1 parts by mass or more, more preferably 5 parts by mass or more, more preferably 10 parts by mass or more, more preferably 25 parts by mass or more, more preferably 40 parts by mass or more, more preferably 100 parts by mass or more, and even more preferably 150 parts by mass or more, relative to 100 parts by mass of the non-conductive polymer. The upper limit is preferably 600 parts by mass or less, more preferably 400 parts by mass or less, more preferably 240 parts by mass or less, and even more preferably 200 parts by mass or less. The carbon particle content is preferably 0.1 parts by mass or more and 600 parts by mass or less, more preferably 25 parts by mass or more and 400 parts by mass or less, more preferably 40 parts by mass or more and 240 parts by mass or less, more preferably 100 parts by mass or more and 200 parts by mass or less, relative to 100 parts by mass of the non-conductive polymer. When the carbon particle content is 0.1 parts by mass or more, conductive paths are easily formed, and sufficient conductivity is easily obtained. Furthermore, if the content of the carbon particles is 600 parts by mass or less, an increase in viscosity of the conductive paste can be suppressed, resulting in excellent coatability. When the conductive filler is silver particles, the lower limit of the content of the silver particles is preferably 50 parts by mass or more, more preferably 60 parts by mass or more, more preferably 70 parts by mass or more, more preferably 100 parts by mass or more, more preferably 150 parts by mass or more, and even more preferably 300 parts by mass or more, relative to 100 parts by mass of the non-conductive polymer.The upper limit is preferably 9,900 parts by mass or less, and may be 1,900 parts by mass or less, 900 parts by mass or less, 500 parts by mass or less, 300 parts by mass or less, or 100 parts by mass or less. The content of the silver particles is preferably 50 parts by mass or more and 9,900 parts by mass or less, more preferably 50 parts by mass or more and 1,900 parts by mass or less, more preferably 70 parts by mass or more and 900 parts by mass or less, more preferably 70 parts by mass or more and 500 parts by mass or less, more preferably 70 parts by mass or more and 300 parts by mass or less, and even more preferably 70 parts by mass or more and 100 parts by mass or less, relative to 100 parts by mass of the non-conductive polymer. When the content of the silver particles is 50 parts by mass or more, conductive paths are easily formed, and sufficient conductivity is easily obtained. Furthermore, when the content of the silver particles is 9,900 parts by mass or less, an increase in the viscosity of the conductive paste can be suppressed, resulting in excellent coatability.
[0047] Even when the resin component according to the embodiment of the present invention is a non-conductive polymer, the conductive layer (which may be a conductive paste) may contain the various additives described above in a content range that achieves the effects of the present invention.
[0048] Examples of crosslinking agents include isocyanate-based crosslinking agents, carbodiimide-based crosslinking agents, epoxy-based crosslinking agents, melamine-based crosslinking agents, peroxide-based crosslinking agents, urea-based crosslinking agents, metal alkoxide-based crosslinking agents, metal chelate-based crosslinking agents, metal salt-based crosslinking agents, oxazoline-based crosslinking agents, aziridine-based crosslinking agents, and amine-based crosslinking agents. Examples of isocyanate-based crosslinking agents include blocked isocyanate, toluene diisocyanate, and methylene bisphenyl isocyanate. Examples of epoxy-based crosslinking agents include N,N,N',N'-tetraglycidyl-m-xylylene diamine, diglycidyl aniline, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, and 1,6-hexanediol diglycidyl ether. When a crosslinking agent is contained, the content is preferably 0.01 to 20 parts by mass per 100 parts by mass of the resin component. The upper limit is more preferably 10 parts by mass, and even more preferably 8 parts by mass. The lower limit is more preferably 1 part by mass, and even more preferably 2 parts by mass. The crosslinking agents can be used alone or in combination of two or more.
[0049] A crosslinking catalyst may be used to more effectively promote the crosslinking reaction. A preferred example of the crosslinking catalyst is a tin-based catalyst (especially dioctyltin dilaurate). The amount of the crosslinking catalyst used is not particularly limited, but may be, for example, 0.0001 to 5 parts by mass per 100 parts by mass of the resin component.
[0050] The thickness of the conductive layer 3 according to the embodiment of the present invention is preferably 0.001 μm or more and 1000 μm or less. The upper limit of the thickness is more preferably 500 μm, even more preferably 300 μm, even more preferably 100 μm, even more preferably 50 μm, even more preferably 10 μm, even more preferably 5 μm, even more preferably 2 μm, even more preferably 1 μm, even more preferably 0.5 μm, and the lower limit is more preferably 0.01 μm, even more preferably 0.02 μm, even more preferably 0.03 μm, even more preferably 0.04 μm, even more preferably 0.05 μm.
[0051] The surface resistance of the conductive layer according to the embodiment of the present invention may be 7000 Ω / □ or less, and preferably 5000 Ω / □ or less. By having the surface resistance of the conductive layer according to the embodiment of the present invention be 5000 Ω / □ or less, excellent conductivity can be obtained. The lower limit of the surface resistance of the conductive layer according to the embodiment of the present invention may be 0.001 Ω / □ or more, 0.01 Ω / □ or more, 0.1 Ω / □ or more, 1 Ω / □ or more, 10 Ω / □ or more, or 100 Ω / □ or more. The upper limit is preferably 3000 Ω / □ or less, more preferably 2000 Ω / □ or less, more preferably 1000 Ω / □ or less, more preferably 500 Ω / □ or less, more preferably 200 Ω / □ or less, and even more preferably 150 Ω / □ or less. The surface resistance of the conductive layer according to the embodiment of the present invention can be measured by the method described in the examples.
[0052] The support substrate 4 according to the embodiment of the present invention is not particularly limited, but examples thereof include paper-based substrates such as paper, fiber-based substrates such as cloth and nonwoven fabric, plastic-based substrates such as films and sheets made of various plastics (polyolefin-based resins such as polyethylene and polypropylene, polyester-based resins such as polyethylene terephthalate, acrylic resins such as polymethyl methacrylate, etc.), and laminates thereof. The substrate may have a single layer structure or a multi-layer structure. The substrate may be subjected to various treatments such as back surface treatment, antistatic treatment, and primer treatment as necessary.
[0053] The thickness of the support substrate 4 according to the embodiment of the present invention can be any thickness depending on the purpose. For example, a thickness of 10 μm or more and 1000 μm or less is preferable. The upper limit of the thickness is more preferably 500 μm, and even more preferably 300 μm, and the lower limit is more preferably 12 μm, and even more preferably 25 μm.
[0054] The conductive substrate 5 according to the embodiment of the present invention is not particularly limited as long as it includes a support substrate 4 and a conductive layer 3 containing a resin component. Examples of the conductive substrate 5 include a substrate in which a conductive layer is formed on the surface of the support substrate 4, and examples thereof include a substrate in which a conductive layer is formed by applying a conductive layer-forming composition containing a resin component to the surface of the support substrate exemplified above, and then heating and / or curing the composition to form the conductive layer.
[0055] The thickness of the conductive substrate 5 according to the embodiment of the present invention can be any thickness depending on the purpose. For example, the thickness is preferably 10 μm or more and 1000 μm or less. The upper limit of the thickness is more preferably 500 μm, and the lower limit is more preferably 12 μm, and even more preferably 25 μm.
[0056] The electrically peelable pressure-sensitive adhesive sheet according to an embodiment of the present invention can be attached to a conductive material to form a bonded body. Examples of conductive materials include adherends such as metal surfaces. Examples of metal surfaces include surfaces made of metals primarily composed of aluminum, copper, iron, magnesium, tin, gold, silver, and lead, with aluminum being preferred. Examples of adherends having a metal surface include sheets, parts, and plates made of metals primarily composed of aluminum, copper, iron, magnesium, tin, gold, silver, and lead. Adherends other than those having a metal surface include, but are not limited to, fiber sheets such as paper, cloth, and nonwoven fabric, as well as various plastic films and sheets.
[0057] The electrically releasing pressure-sensitive adhesive layer 1 is a pressure-sensitive adhesive layer whose adhesive strength decreases upon application of a voltage. The electrically releasing pressure-sensitive adhesive layer contains a polymer as an adhesive and an electrolyte. The electrolyte contained in the electrically releasing pressure-sensitive adhesive layer is a substance that can be ionized into anions and cations. Examples of such electrolytes include ionic liquids, alkali metal salts, and alkaline earth metal salts. From the perspective of achieving good electrical peelability in the electrically releasing pressure-sensitive adhesive layer, an ionic liquid is preferred as the electrolyte contained in the electrically releasing pressure-sensitive adhesive layer. An ionic liquid is a salt that is liquid at room temperature (approximately 25°C) and contains anions and cations. That is, the electrically releasing pressure-sensitive adhesive layer preferably contains a polymer and an ionic liquid. The electrically releasing pressure-sensitive adhesive layer 1 can be formed from a pressure-sensitive adhesive composition containing a polymer and an ionic liquid. The pressure-sensitive adhesive composition according to an embodiment of the present invention will be described below. Note that, in this specification, the adhesive strength when no voltage is applied may be referred to as "initial adhesive strength." Furthermore, a composition containing components other than the ionic liquid among the components contained in the pressure-sensitive adhesive composition may be referred to as an "ionic liquid-free pressure-sensitive adhesive composition." A pressure-sensitive adhesive layer formed from an ionic liquid-free pressure-sensitive adhesive composition is sometimes referred to as an “ionic liquid-free pressure-sensitive adhesive layer.” The property of adhesive strength decreasing upon voltage application is sometimes referred to as “electrical peeling property,” and a large rate of decrease in adhesive strength upon voltage application is sometimes referred to as “excellent electrical peeling property.”
[0058] <Components of Pressure-Sensitive Adhesive Composition> (Polymer) The pressure-sensitive adhesive composition according to the embodiment of the present invention contains a polymer. In the present embodiment, the polymer is not particularly limited as long as it is a general organic polymer compound, and is, for example, a polymer or partial polymer of a monomer. The monomer may be one type of monomer or a mixture of two or more types of monomers. Note that a partial polymer refers to a polymer in which at least a part of the monomer or monomer mixture is partially polymerized.
[0059] The polymer in this embodiment is not particularly limited as long as it is typically used as a pressure-sensitive adhesive and has adhesive properties, but examples include acrylic polymers, rubber polymers, vinyl alkyl ether polymers, silicone polymers, polyester polymers, polyamide polymers, urethane polymers, fluorine-based polymers, and epoxy polymers. The polymers can be used alone or in combination of two or more. In order to increase the dielectric constant of the components other than the ionic liquid in the resulting electrically peelable pressure-sensitive adhesive layer and improve the electrical peelability, it is preferable that the polymer have a high dielectric constant. From this perspective, it is particularly preferable that the polymer in this embodiment includes at least one selected from the group consisting of polyester polymers and acrylic polymers having carboxyl groups and / or hydroxyl groups. Because polyester polymers have easily polarizable hydroxyl groups at their terminals, and because acrylic polymers having carboxyl groups and / or hydroxyl groups have easily polarizable carboxyl groups and / or hydroxyl groups, the use of these polymers can produce polymers with relatively high dielectric constants. The total content of the polyester polymer and the acrylic polymer having a carboxyl group and / or a hydroxyl group in the polymer according to the embodiment of the present invention is preferably 60% by mass or more, more preferably 80% by mass or more. Furthermore, particularly for improving costs, productivity, and initial adhesive strength, the polymer according to the present embodiment is preferably an acrylic polymer. That is, the pressure-sensitive adhesive composition according to the embodiment of the present invention is preferably an acrylic pressure-sensitive adhesive composition containing an acrylic polymer as the polymer.
[0060] The acrylic polymer preferably contains a monomer unit derived from a (meth)acrylic acid alkyl ester (the following formula (1)) having an alkyl group having 1 to 14 carbon atoms. Such a monomer unit is suitable for obtaining a large initial adhesive strength. In addition, in order to increase the relative dielectric constant of the components of the electrically peelable pressure-sensitive adhesive layer other than the ionic liquid and improve the electrical peelability, the alkyl group R bThe number of carbon atoms in is preferably small, particularly preferably 8 or less, and more preferably 4 or less. 2 = C(R a ) COOR b (1) [R in formula (1)] a is a hydrogen atom or a methyl group, and R b is an alkyl group having 1 to 14 carbon atoms which may have a substituent.
[0061] Examples of (meth)acrylic acid alkyl esters having an alkyl group having 1 to 14 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, 1,3-dimethylbutyl acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, and 2-ethylbutyl (meth)acrylate. acrylate, heptyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl (meth)acrylate, n-dodecyl (meth)acrylate, n-tridecyl (meth)acrylate, n-tetradecyl (meth)acrylate, and 2-methoxyethyl acrylate. Of these, n-butyl acrylate, 2-ethylhexyl acrylate, isononyl acrylate, and 2-methoxyethyl acrylate are preferred. The (meth)acrylic acid alkyl esters having an alkyl group having 1 to 14 carbon atoms can be used alone or in combination of two or more.
[0062] The proportion of the (meth)acrylic acid alkyl ester having an alkyl group having 1 to 14 carbon atoms relative to all monomer components (100% by mass) constituting the acrylic polymer is not particularly limited, but is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 85% by mass or more. When the proportion of the (meth)acrylic acid alkyl ester having an alkyl group having 1 to 14 carbon atoms is 70% by mass or more, a large initial adhesive strength is easily obtained.
[0063] For the purpose of improving cohesive strength, heat resistance, crosslinkability, etc., the acrylic polymer preferably contains a monomer unit derived from a polar group-containing monomer copolymerizable with a (meth)acrylic acid alkyl ester having an alkyl group having 1 to 14 carbon atoms, in addition to the monomer unit. Such a monomer unit can impart crosslinking points and is suitable for obtaining high initial adhesive strength. Furthermore, from the viewpoint of increasing the relative permittivity of components other than the ionic liquid in the electrically peelable pressure-sensitive adhesive layer and improving electrical peelability, it is also preferable to contain a monomer unit derived from a polar group-containing monomer.
[0064] Examples of polar group-containing monomers include carboxyl group-containing monomers, hydroxyl group-containing monomers, cyano group-containing monomers, vinyl group-containing monomers, aromatic vinyl monomers, amide group-containing monomers, imide group-containing monomers, amino group-containing monomers, epoxy group-containing monomers, vinyl ether monomers, N-acryloylmorpholine, sulfo group-containing monomers, phosphate group-containing monomers, and acid anhydride group-containing monomers. Among these, carboxyl group-containing monomers, hydroxyl group-containing monomers, and amide group-containing monomers are preferred from the viewpoint of excellent cohesiveness, and carboxyl group-containing monomers are particularly preferred. Carboxyl group-containing monomers are particularly suitable for obtaining high initial adhesive strength. Polar group-containing monomers can be used alone or in combination of two or more.
[0065] Examples of carboxyl group-containing monomers include acrylic acid, methacrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, and isocrotonic acid. Acrylic acid is particularly preferred. The carboxyl group-containing monomers can be used alone or in combination.
[0066] Examples of hydroxyl group-containing monomers include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, (4-hydroxymethylcyclohexyl)methyl (meth)acrylate, N-methylol (meth)acrylamide, vinyl alcohol, allyl alcohol, 2-hydroxyethyl vinyl ether, 4-hydroxybutyl vinyl ether, and diethylene glycol monovinyl ether. 2-Hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate are particularly preferred. The hydroxyl group-containing monomers may be used alone or in combination of two or more.
[0067] Examples of amide group-containing monomers include acrylamide, methacrylamide, N-vinylpyrrolidone, N,N-dimethylacrylamide, N,N-dimethylmethacrylamide, N,N-diethylacrylamide, N,N-diethylmethacrylamide, N,N'-methylenebisacrylamide, N,N-dimethylaminopropylacrylamide, N,N-dimethylaminopropylmethacrylamide, and diacetoneacrylamide. The amide group-containing monomers can be used alone or in combination of two or more.
[0068] Examples of cyano group-containing monomers include acrylonitrile and methacrylonitrile.
[0069] Examples of vinyl group-containing monomers include vinyl esters such as vinyl acetate, vinyl propionate, and vinyl laurate, with vinyl acetate being particularly preferred.
[0070] Examples of aromatic vinyl monomers include styrene, chlorostyrene, chloromethylstyrene, α-methylstyrene, and other substituted styrenes.
[0071] Examples of imide group-containing monomers include cyclohexylmaleimide, isopropylmaleimide, N-cyclohexylmaleimide, and itaconimide.
[0072] Examples of amino group-containing monomers include aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, and N,N-dimethylaminopropyl (meth)acrylate.
[0073] Examples of epoxy group-containing monomers include glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, and allyl glycidyl ether.
[0074] Examples of vinyl ether monomers include methyl vinyl ether, ethyl vinyl ether, and isobutyl vinyl ether.
[0075] The proportion of the polar group-containing monomer relative to the total monomer components (100% by mass) constituting the acrylic polymer is preferably 0.1% by mass or more and 35% by mass or less. The upper limit of the polar group-containing monomer proportion is more preferably 25% by mass, even more preferably 20% by mass, and the lower limit is more preferably 0.5% by mass, even more preferably 1% by mass, and particularly preferably 2% by mass. When the proportion of the polar group-containing monomer is 0.1% by mass or more, cohesive strength is easily obtained, so that adhesive residue is less likely to remain on the adherend surface after peeling the electrically-release pressure-sensitive adhesive layer, and the electrical releasability is improved. Furthermore, when the proportion of the polar group-containing monomer is 30% by mass or less, it is easy to prevent the electrically-release pressure-sensitive adhesive layer from excessively adhering to the adherend and causing heavy peeling. In particular, when the proportion is 2% by mass or more and 20% by mass or less, it is easy to achieve both releasability from the adherend and adhesion between the electrically-release pressure-sensitive adhesive layer and the conductive layer.
[0076] Furthermore, the monomer components constituting the acrylic polymer may contain a polyfunctional monomer in order to introduce a crosslinked structure into the acrylic polymer and make it easier to obtain the required cohesive strength.
[0077] Examples of polyfunctional monomers include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, divinylbenzene, and N,N'-methylenebisacrylamide. The polyfunctional monomers can be used alone or in combination of two or more.
[0078] The content of the polyfunctional monomer relative to the total monomer components (100% by mass) constituting the acrylic polymer is preferably 0.1% by mass or more and 15% by mass or less. The upper limit of the polyfunctional monomer content is more preferably 10% by mass, and the lower limit is more preferably 3% by mass. When the content of the polyfunctional monomer is 0.1% by mass or more, the flexibility and adhesiveness of the electrically peelable pressure-sensitive adhesive layer are easily improved, which is preferable. When the content of the polyfunctional monomer is 15% by mass or less, the cohesive force is not too high, and appropriate adhesiveness is easily obtained.
[0079] Polyester-based polymers are typically polymers having a structure formed by condensation of a polycarboxylic acid such as a dicarboxylic acid or a derivative thereof (hereinafter also referred to as a "polycarboxylic acid monomer") with a polyhydric alcohol such as a diol or a derivative thereof (hereinafter referred to as a "polyhydric alcohol monomer").
[0080] The polycarboxylic acid monomer is not particularly limited, but examples thereof include adipic acid, azelaic acid, dimer acid, sebacic acid, 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, 4-methyl-1,2-cyclohexanedicarboxylic acid, dodecenylsuccinic anhydride, fumaric acid, succinic acid, dodecanedioic acid, hexahydrophthalic anhydride, tetrahydrophthalic anhydride, maleic acid, maleic anhydride, itaconic acid, citraconic acid, and derivatives thereof. The polycarboxylic acid monomers can be used alone or in combination of two or more.
[0081] The polyhydric alcohol monomer is not particularly limited, but examples thereof include ethylene glycol, 1,2-propylene glycol, 1,3-propanediol, 2-methyl-1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, neopentyl glycol, diethylene glycol, dipropylene glycol, 2,2,4-trimethyl-1,5-pentanediol, 2-ethyl-2-butylpropanediol, 1,9-nonanediol, 2-methyloctanediol, 1,10-decanediol, and derivatives thereof. The polyhydric alcohol monomers can be used alone or in combination of two or more.
[0082] Furthermore, the polymer according to the embodiment of the present invention may contain an ionic polymer. The ionic polymer is a polymer having an ionic functional group. When the polymer contains the ionic polymer, the relative dielectric constant of the polymer increases, and the electrodetachment property is improved. When the polymer contains the ionic polymer, the content of the ionic polymer is preferably 0.05 parts by mass or more and 2 parts by mass or less per 100 parts by mass of the polymer.
[0083] In this embodiment, the polymer can be obtained by (co)polymerizing monomer components. The polymerization method is not particularly limited, but examples thereof include solution polymerization, emulsion polymerization, bulk polymerization, suspension polymerization, and photopolymerization (active energy ray polymerization). In particular, from the viewpoints of cost and productivity, solution polymerization is preferred. When copolymerized, the polymer may be any of a random copolymer, a block copolymer, an alternating copolymer, a graft copolymer, and the like.
[0084] The solution polymerization method is not particularly limited, but examples thereof include a method in which a monomer component, a polymerization initiator, etc. are dissolved in a solvent and heated to polymerize, thereby obtaining a polymer solution containing a polymer.
[0085] As the solvent used in the solution polymerization method, various common solvents can be used. Examples of such solvents (polymerization solvents) include organic solvents such as aromatic hydrocarbons such as toluene, benzene, and xylene; esters such as ethyl acetate and n-butyl acetate; aliphatic hydrocarbons such as n-hexane and n-heptane; alicyclic hydrocarbons such as cyclohexane and methylcyclohexane; and ketones such as methyl ethyl ketone and methyl isobutyl ketone. The solvents can be used alone or in combination of two or more.
[0086] The amount of the solvent used is not particularly limited, but is preferably 10 parts by mass or more and 1,000 parts by mass or less relative to the total monomer components (100 parts by mass) constituting the polymer. The upper limit of the amount of the solvent used is more preferably 500 parts by mass, and the lower limit is more preferably 50 parts by mass.
[0087] The polymerization initiator used in the solution polymerization method is not particularly limited, but examples thereof include peroxide-based polymerization initiators, azo-based polymerization initiators, etc. Examples of the peroxide-based polymerization initiator are not particularly limited, but examples thereof include peroxycarbonate, ketone peroxide, peroxyketal, hydroperoxide, dialkyl peroxide, diacyl peroxide, and peroxyester, and more specific examples thereof include benzoyl peroxide, t-butyl hydroperoxide, di-t-butyl peroxide, t-butyl peroxybenzoate, dicumyl peroxide, 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexane, and 1,1-bis(t-butylperoxy)cyclododecane, etc. The azo polymerization initiator is not particularly limited, but examples thereof include 2,2'-azobisisobutyronitrile, 2,2'-azobis-2-methylbutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2-methylpropionate)dimethyl, 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis(2,4,4-trimethylpentane), 4,4'-azobis Examples of polymerization initiators include 4-cyanovaleric acid, 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis[2-(5-methyl-2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis(2-methylpropionamidine) disulfate, 2,2'-azobis(N,N'-dimethyleneisobutylamidine) hydrochloride, and 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] hydrate. The polymerization initiators can be used alone or in combination of two or more.
[0088] The amount of the polymerization initiator used is not particularly limited, but is preferably 0.01 to 5 parts by mass relative to the total monomer components (100 parts by mass) constituting the polymer. The upper limit of the amount of the polymerization initiator used is more preferably 3 parts by mass, and the lower limit is more preferably 0.05 parts by mass.
[0089] In the solution polymerization method, the heating temperature when polymerizing by heating is not particularly limited, but is, for example, 50° C. to 80° C. The heating time is not particularly limited, but is, for example, 1 hour to 24 hours.
[0090] The weight-average molecular weight of the polymer is not particularly limited, but is preferably 100,000 or more and 5,000,000 or less. The upper limit of the weight-average molecular weight is more preferably 4,000,000, even more preferably 3,000,000, and the lower limit is more preferably 200,000, even more preferably 300,000. When the weight-average molecular weight is 100,000 or more, the cohesive force is reduced, and the problem of adhesive residue remaining on the adherend surface after peeling off the electrically-peeling pressure-sensitive adhesive layer can be effectively suppressed. Furthermore, when the weight-average molecular weight is 5,000,000 or less, the problem of insufficient wettability on the adherend surface after peeling off the electrically-peeling pressure-sensitive adhesive layer can be effectively suppressed.
[0091] The weight-average molecular weight is obtained by measurement by gel permeation chromatography (GPC). More specifically, for example, measurement is performed using a GPC measurement device under the trade name "HLC-8220GPC" (manufactured by Tosoh Corporation) under the following conditions, and the weight-average molecular weight can be calculated in terms of a standard polystyrene. (Weight-average molecular weight measurement conditions) Sample concentration: 0.2% by mass (tetrahydrofuran solution) Sample injection amount: 10 μL Sample column: TSKguard column SuperHZ-H (1 column) + TSKgel SuperHZM-H (2 columns) Reference column: TSKgel SuperH-RC (1 column) Eluent: tetrahydrofuran (THF) Flow rate: 0.6 mL / min Detector: differential refractometer (RI) Column temperature (measurement temperature): 40°C
[0092] The glass transition temperature (Tg) of the polymer is not particularly limited, but is preferably 0° C. or lower because this can suppress a decrease in the initial adhesive strength, more preferably −10° C. or lower, and even more preferably −20° C. or lower. Furthermore, if it is −40° C. or lower, the rate of decrease in adhesive strength due to voltage application becomes particularly large, so it is particularly preferred, and most preferably −50° C. or lower.
[0093] The glass transition temperature (Tg) can be calculated, for example, based on the following formula (Y) (Fox formula): 1 / Tg=W1 / Tg1+W2 / Tg2+ ... +Wn / Tgn (Y) [In formula (Y), Tg is the glass transition temperature (unit: K) of the polymer, Tgi (i = 1, 2, ... n) is the glass transition temperature (unit: K) when monomer i forms a homopolymer, and Wi (i = 1, 2, ... n) is the mass fraction of monomer i in all monomer components] The above formula (Y) is a calculation formula when a polymer is composed of n types of monomer components, i.e., monomer 1, monomer 2, ..., monomer n.
[0094] The glass transition temperature when a homopolymer is formed refers to the glass transition temperature of a homopolymer of the monomer, and refers to the glass transition temperature (Tg) of a polymer formed using only a certain monomer (sometimes referred to as "monomer X") as the monomer component. Specific values are listed in "Polymer Handbook" (3rd Edition, John Wiley & Sons, Inc., 1989). The glass transition temperature (Tg) of a homopolymer not described in this document refers to a value obtained, for example, by the following measurement method. Specifically, 100 parts by mass of monomer X, 0.2 parts by mass of 2,2'-azobisisobutyronitrile, and 200 parts by mass of ethyl acetate as a polymerization solvent are placed in a reactor equipped with a thermometer, a stirrer, a nitrogen inlet tube, and a reflux condenser, and the mixture is stirred for 1 hour while introducing nitrogen gas. After removing oxygen from the polymerization system in this way, the temperature is raised to 63°C and the reaction is allowed to proceed for 10 hours. The mixture is then cooled to room temperature to obtain a homopolymer solution with a solids concentration of 33% by mass. Next, this homopolymer solution is cast onto a release liner and dried to prepare a test sample (sheet-like homopolymer) with a thickness of approximately 2 mm. Approximately 1 to 2 mg of this test sample is weighed into an aluminum open cell, and the reversing heat flow (specific heat component) behavior of the homopolymer is measured using a temperature-modulated DSC (trade name "Q-2000" manufactured by TA Instruments) at a heating rate of 5°C / min under a nitrogen atmosphere of 50 ml / min. With reference to JIS-K-7121, the glass transition temperature (Tg) of the homopolymer is determined as the temperature at the point where a line equidistant in the vertical direction from a line extending the low-temperature baseline and the high-temperature baseline of the obtained reversing heat flow intersects with the curve representing the stepwise change in the glass transition.
[0095] The polymer content in the pressure-sensitive adhesive composition according to the embodiment of the present invention is preferably 50% by mass or more and 99.9% by mass or less, relative to the total amount (100% by mass) of the pressure-sensitive adhesive composition, the upper limit is more preferably 99.5% by mass, and even more preferably 99% by mass, and the lower limit is more preferably 60% by mass, and even more preferably 70% by mass.
[0096] (Ionic Liquid) The ionic liquid in this embodiment is not particularly limited as long as it is a molten salt (room-temperature molten salt) composed of a pair of anion and cation and is liquid at 25° C. Examples of anions and cations are given below, but among the ionic substances obtained by combining these, those that are liquid at 25° C. are ionic liquids, and those that are solid at 25° C. are not ionic liquids but are ionic solids described below.
[0097] The anion of the ionic liquid is, for example, (FSO 2 ) 2 N - , (CF 3 SO 2 ) 2 N - , (CF 3 CF 2 SO 2 ) 2 N - , (CF 3 SO 2 ) 3 C - ,Br - , AlCl 4 - , Al 2 Cl 7 - , NO 3 - , B.F. 4 - , P.F. 6 - , C.H. 3 COO - , C.F. 3 COO - , C.F. 3 CF 2 CF 2 COO - , C.F. 3 SO 3 - , C.F. 3 (CF 2 ) 3 SO 3 - , AsF 6 - , SbF 6 - , and F(HF) n -Among them, the anion is (FSO 2 ) 2 N - [bis(fluorosulfonyl)imide anion], and (CF 3 SO 2 ) 2 N - Anions of sulfonylimide compounds such as bis(trifluoromethanesulfonyl)imide anions are preferred because they are chemically stable and suitable for improving electrical peelability. That is, the anion of the ionic liquid is preferably at least one selected from the group consisting of bis(fluorosulfonyl)imide anions and bis(trifluoromethanesulfonyl)imide anions.
[0098] The cation in the ionic liquid is preferably at least one selected from the group consisting of nitrogen-containing onium cations, sulfur-containing onium cations, and phosphorus-containing onium cations, as these are chemically stable and suitable for improving electrical peelability, and imidazolium-based, ammonium-based, pyrrolidinium-based, and pyridinium-based cations are more preferred.
[0099] Examples of imidazolium cations include 1-methylimidazolium cation, 1-ethyl-3-methylimidazolium cation, 1-propyl-3-methylimidazolium cation, 1-butyl-3-methylimidazolium cation, 1-pentyl-3-methylimidazolium cation, 1-hexyl-3-methylimidazolium cation, 1-heptyl-3-methylimidazolium cation, 1-octyl-3-methylimidazolium cation, 1-nonyl-3-methylimidazolium cation, 1-undecyl-3-methylimidazolium cation, and 1-dodecyl-3-methylimidazolium cation. imidazolium cation, 1-tridecyl-3-methylimidazolium cation, 1-tetradecyl-3-methylimidazolium cation, 1-pentadecyl-3-methylimidazolium cation, 1-hexadecyl-3-methylimidazolium cation, 1-heptadecyl-3-methylimidazolium cation, 1-octadecyl-3-methylimidazolium cation, 1-undecyl-3-methylimidazolium cation, 1-benzyl-3-methylimidazolium cation, 1-butyl-2,3-dimethylimidazolium cation, and 1,3-bis(dodecyl)imidazolium cation.
[0100] Examples of pyridinium cations include 1-butylpyridinium cation, 1-hexylpyridinium cation, 1-butyl-3-methylpyridinium cation, 1-butyl-4-methylpyridinium cation, and 1-octyl-4-methylpyridinium cation.
[0101] Examples of pyrrolidinium cations include 1-ethyl-1-methylpyrrolidinium cation and 1-butyl-1-methylpyrrolidinium cation.
[0102] Examples of ammonium-based cations include tetraethylammonium cation, tetrabutylammonium cation, methyltrioctylammonium cation, tetradecyltrihexylammonium cation, glycidyltrimethylammonium cation, and trimethylaminoethylacrylate cation.
[0103] From the viewpoint of increasing the rate of decrease in adhesive strength when a voltage is applied, it is preferable to select a cation having a molecular weight of 160 or less as the constituent cation of the ionic liquid. 2 ) 2 N - [bis(fluorosulfonyl)imide anion] or (CF 3 SO 2 ) 2 N - Particularly preferred is an ionic liquid containing a bis(trifluoromethanesulfonyl)imide anion and a cation having a molecular weight of 160 or less. Examples of the cation having a molecular weight of 160 or less include a 1-methylimidazolium cation, a 1-ethyl-3-methylimidazolium cation, a 1-propyl-3-methylimidazolium cation, a 1-butyl-3-methylimidazolium cation, a 1-pentyl-3-methylimidazolium cation, a 1-butylpyridinium cation, a 1-hexylpyridinium cation, a 1-butyl-3-methylpyridinium cation, a 1-butyl-4-methylpyridinium cation, a 1-ethyl-1-methylpyrrolidinium cation, a 1-butyl-1-methylpyrrolidinium cation, a tetraethylammonium cation, a glycidyltrimethylammonium cation, and a trimethylaminoethyl acrylate cation.
[0104] Furthermore, as the cation of the ionic liquid, cations represented by the following formulas (2-A) to (2-D) are also preferred.
[0105]
[0106] R in formula (2-A) 1 represents a hydrocarbon group having 4 to 10 carbon atoms (preferably a hydrocarbon group having 4 to 8 carbon atoms, more preferably a hydrocarbon group having 4 to 6 carbon atoms), which may contain a heteroatom; R 2 and R 3are the same or different and represent a hydrogen atom or a hydrocarbon group having 1 to 12 carbon atoms (preferably a hydrocarbon group having 1 to 8 carbon atoms, more preferably a hydrocarbon group having 2 to 6 carbon atoms, and even more preferably a hydrocarbon group having 2 to 4 carbon atoms), and may contain a heteroatom. However, when a nitrogen atom forms a double bond with an adjacent carbon atom, R 3 does not exist.
[0107] R in formula (2-B) 4 represents a hydrocarbon group having 2 to 10 carbon atoms (preferably a hydrocarbon group having 2 to 8 carbon atoms, more preferably a hydrocarbon group having 2 to 6 carbon atoms), which may contain a heteroatom; R 5 , R 6 , and R 7 are the same or different and represent a hydrogen atom or a hydrocarbon group having 1 to 12 carbon atoms (preferably a hydrocarbon group having 1 to 8 carbon atoms, more preferably a hydrocarbon group having 2 to 6 carbon atoms, and even more preferably a hydrocarbon group having 2 to 4 carbon atoms), which may contain a heteroatom.
[0108] R in formula (2-C) 8 represents a hydrocarbon group having 2 to 10 carbon atoms (preferably a hydrocarbon group having 2 to 8 carbon atoms, more preferably a hydrocarbon group having 2 to 6 carbon atoms), which may contain a heteroatom; R 9 , R 10 , and R 11 are the same or different and represent a hydrogen atom or a hydrocarbon group having 1 to 16 carbon atoms (preferably a hydrocarbon group having 1 to 10 carbon atoms, more preferably a hydrocarbon group having 1 to 8 carbon atoms), which may contain a heteroatom.
[0109] In formula (2-D), X represents a nitrogen, sulfur, or phosphorus atom; 12 , R 13 , R 14 , and R 15 are the same or different and represent a hydrocarbon group having 1 to 16 carbon atoms (preferably a hydrocarbon group having 1 to 14 carbon atoms, more preferably a hydrocarbon group having 1 to 10 carbon atoms, even more preferably a hydrocarbon group having 1 to 8 carbon atoms, and particularly preferably a hydrocarbon group having 1 to 6 carbon atoms), which may contain a heteroatom. However, when X is a sulfur atom, R 12 does not exist.
[0110] The molecular weight of the cation in the ionic liquid is, for example, 500 or less, preferably 400 or less, more preferably 300 or less, even more preferably 250 or less, particularly preferably 200 or less, and most preferably 160 or less. It is usually 50 or more. It is believed that the cation in the ionic liquid has the property of migrating to the cathode side in the electrically releasing pressure-sensitive adhesive layer upon application of a voltage, and being biased toward the interface between the electrically releasing pressure-sensitive adhesive layer and the adherend. For this reason, in the present invention, the adhesive strength during voltage application decreases relative to the initial adhesive strength, resulting in electro-releasability. Cations with a small molecular weight, such as a molecular weight of 500 or less, are suitable for facilitating the migration of cations to the cathode side in the electrically releasing pressure-sensitive adhesive layer and increasing the rate of decrease in adhesive strength upon application of a voltage.
[0111] Examples of commercially available ionic liquids include "ELEXEL AS-110," "ELEXEL MP-442," "ELEXEL IL-210," "ELEXEL MP-471," "ELEXEL MP-456," and "ELEXEL AS-804" manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.; "HMI-FSI" manufactured by Mitsubishi Materials Corporation; and "CIL-312" and "CIL-313" manufactured by Nippon Carlit Co., Ltd.
[0112] The ionic conductivity is preferably 0.1 mS / cm or more and 20 mS / cm or less. The upper limit of the ionic conductivity is more preferably 18 mS / cm, and the lower limit is more preferably 0.3 mS / cm, more preferably 0.5 mS / cm, more preferably 1 mS / cm, more preferably 5 mS / cm, more preferably 8 mS / cm, and even more preferably 10 mS / cm. By having an ionic conductivity within this range, the adhesive strength is sufficiently reduced even at a low voltage. The ionic conductivity can be measured by an AC impedance method, for example, using a Solartron 1260 frequency response analyzer.
[0113] The content (blending amount) of the ionic liquid in the pressure-sensitive adhesive composition according to the embodiment of the present invention is preferably 0.5 parts by mass or more relative to 100 parts by mass of the polymer from the viewpoint of reducing adhesive strength during voltage application, and preferably 30 parts by mass or less from the viewpoint of increasing initial adhesive strength. From the same viewpoint, it is more preferably 20 parts by mass or less, even more preferably 15 parts by mass or less, particularly preferably 10 parts by mass or less, and most preferably 5 parts by mass or less. Furthermore, it is more preferably 0.6 parts by mass or more, even more preferably 0.8 parts by mass or more, particularly preferably 1.0 parts by mass or more, and most preferably 1.5 parts by mass or more.
[0114] (Other Components) The pressure-sensitive adhesive composition according to the embodiment of the present invention may contain one or more components other than the polymer and the ionic liquid (hereinafter, sometimes referred to as "other components"), as needed, within a range that does not impair the effects of the present invention. Hereinafter, other components that may be contained in the pressure-sensitive adhesive composition according to the embodiment of the present invention will be described.
[0115] The pressure-sensitive adhesive composition according to the embodiment of the present invention may contain an ionic additive. As the ionic additive, for example, an ionic solid can be used.
[0116] The ionic solid is an ionic substance that is solid at 25° C. There are no particular limitations on the ionic solid, and for example, a solid ionic substance obtained by combining an anion and a cation as exemplified in the section describing the ionic liquid above can be used. When the pressure-sensitive adhesive composition contains an ionic solid, the content of the ionic solid is preferably 0.5 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the polymer.
[0117] The pressure-sensitive adhesive composition according to the present invention may contain a crosslinking agent, if necessary, for the purpose of improving creep resistance and shear resistance by crosslinking the polymer. Examples of crosslinking agents include isocyanate-based crosslinking agents, carbodiimide-based crosslinking agents, epoxy-based crosslinking agents, melamine-based crosslinking agents, peroxide-based crosslinking agents, urea-based crosslinking agents, metal alkoxide-based crosslinking agents, metal chelate-based crosslinking agents, metal salt-based crosslinking agents, oxazoline-based crosslinking agents, aziridine-based crosslinking agents, and amine-based crosslinking agents. Examples of isocyanate-based crosslinking agents include toluene diisocyanate and methylene bisphenyl isocyanate. Examples of epoxy-based crosslinking agents include N,N,N',N'-tetraglycidyl-m-xylylene diamine, diglycidyl aniline, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, and 1,6-hexanediol diglycidyl ether. When a crosslinking agent is contained, the content thereof is preferably 0.1 parts by mass or more and 50 parts by mass or less relative to 100 parts by mass of the polymer. The crosslinking agents may be used alone or in combination of two or more.
[0118] The pressure-sensitive adhesive composition according to the embodiment of the present invention may contain polyethylene glycol, if necessary, to aid the movement of the ionic liquid when a voltage is applied. As the polyethylene glycol, one having a number average molecular weight of 200 to 6000 can be used. When polyethylene glycol is contained, the content is preferably 0.1 parts by mass or more and 30 parts by mass or less per 100 parts by mass of the polymer.
[0119] The pressure-sensitive adhesive composition according to the embodiment of the present invention may contain a conductive filler, if necessary, for the purpose of imparting electrical conductivity to the pressure-sensitive adhesive composition. The conductive filler is not particularly limited, and a commonly known or commonly used conductive filler can be used, such as graphite, carbon black, carbon fiber, or metal powder such as silver or copper. When a conductive filler is contained, the content thereof is preferably 0.1 parts by mass or more and 200 parts by mass or less relative to 100 parts by mass of the polymer.
[0120] The pressure-sensitive adhesive composition according to the embodiment of the present invention may also contain various additives such as fillers, plasticizers, antioxidants, antioxidants, pigments (dyes), flame retardants, solvents, surfactants (leveling agents), rust inhibitors, adhesion-imparting resins, corrosion inhibitors, and antistatic agents. The total content of these components is not particularly limited as long as the effects of the present invention are achieved, but is preferably 0.01 parts by mass or more and 20 parts by mass or less, more preferably 10 parts by mass or less, and even more preferably 5 parts by mass or less, per 100 parts by mass of the polymer.
[0121] Examples of fillers include silica, iron oxide, zinc oxide, aluminum oxide, titanium oxide, barium oxide, magnesium oxide, calcium carbonate, magnesium carbonate, zinc carbonate, pyrophyllite clay, kaolin clay, and calcined clay. Examples of plasticizers that can be used include known and commonly used plasticizers used in general resin compositions, such as oils such as paraffin oil and process oil, liquid rubbers such as liquid polyisoprene, liquid polybutadiene, and liquid ethylene-propylene rubber, tetrahydrophthalic acid, azelaic acid, benzoic acid, phthalic acid, trimellitic acid, pyromellitic acid, adipic acid, sebacic acid, fumaric acid, maleic acid, itaconic acid, citric acid, and derivatives thereof, dioctyl phthalate (DOP), dibutyl phthalate (DBP), dioctyl adipate, diisononyl adipate (DINA), and isodecyl succinate. Examples of antioxidants include hindered phenol compounds, aliphatic and aromatic hindered amine compounds, etc. Examples of antioxidants include butylhydroxytoluene (BHT) and butylhydroxyanisole (BHA). Examples of pigments include inorganic pigments such as titanium dioxide, zinc oxide, ultramarine, red iron oxide, lithopone, lead, cadmium, iron, cobalt, aluminum, hydrochloride, and sulfate, as well as organic pigments such as azo pigments and copper phthalocyanine pigments. Examples of rust inhibitors include zinc phosphate, tannic acid derivatives, phosphate esters, basic sulfonates, and various rust-preventive pigments. Examples of adhesion promoters include titanium coupling agents and zirconium coupling agents. Examples of antistatic agents generally include quaternary ammonium salts or hydrophilic compounds such as polyglycolic acid and ethylene oxide derivatives. Examples of tackifying resins include rosin-based tackifying resins, terpene-based tackifying resins, phenol-based tackifying resins, hydrocarbon-based tackifying resins, ketone-based tackifying resins, as well as polyamide-based tackifying resins, epoxy-based tackifying resins, and elastomer-based tackifying resins. These tackifying resins can be used alone or in combination of two or more.Examples of corrosion inhibitors include carbodiimide compounds, adsorption inhibitors, and chelating-type metal deactivators. For example, those described in JP 2019-059908 A can be used.
[0122] <Initial Adhesion Strength, Decrease Rate of Adhesion Strength Due to Voltage Application> The adhesion strength of the electrically peelable pressure-sensitive adhesive layer according to an embodiment of the present invention can be evaluated by various methods, for example, the 180° peel test described in the Examples section.
[0123] The electrically peelable pressure-sensitive adhesive layer according to an embodiment of the present invention is prepared by forming an electrically peelable pressure-sensitive adhesive sheet as described in the Examples section, storing the sheet under high temperature and high humidity conditions for a long period of time, and then carrying out a 180° peel test. The initial adhesive strength (adhesion strength when no voltage is applied) is preferably 2.0 N / cm or more, more preferably 2.5 N / cm or more, and most preferably 3.0 N / cm or more. When the initial adhesive strength is 3.0 N / cm or more, the adhesion to the adherend is sufficient, and the adherend is unlikely to peel off or slip.
[0124] The electrically peelable pressure-sensitive adhesive layer according to the embodiment of the present invention is prepared by forming an electrically peelable pressure-sensitive adhesive sheet as described in the Examples section, storing the sheet under high temperature and high humidity conditions for a long period of time, applying a voltage, and then conducting a 180° peel test. The electrical peel strength measured is preferably 3.0 N / cm or less, more preferably 2.0 N / cm or less. The greater the difference from the initial adhesive strength, the better the electrical peelability is, and the difference from the initial adhesive strength is, for example, preferably 3.0 N / cm or more, more preferably 6.0 N / cm or more.
[0125] The applied voltage is preferably 1 V or more, more preferably 3 V or more, more preferably 5 V or more, more preferably 6 V or more, and even more preferably 10 V or more. It is also preferably 500 V or less, more preferably 300 V or less, even more preferably 100 V or less, and particularly preferably 50 V or less. The voltage application time is preferably 300 seconds or less, more preferably 180 seconds or less, even more preferably 120 seconds or less, even more preferably 60 seconds or less, and particularly preferably 30 seconds or less. In this case, workability is excellent. The shorter the application time, the better, but it is usually 1 second or more.
[0126] The pressure-sensitive adhesive composition according to an embodiment of the present invention is not particularly limited, but can be produced by appropriately stirring and mixing a polymer, an ionic liquid, and additives, such as a crosslinking agent, polyethylene glycol, and a conductive filler, which may be blended as needed.
[0127] From the viewpoint of initial adhesive strength, the thickness of the electrically peeling pressure-sensitive adhesive layer 1 is preferably 1 μm or more and 1,000 μm or less. The upper limit of the thickness of the electrically peeling pressure-sensitive adhesive layer 1 is more preferably 500 μm, even more preferably 300 μm, even more preferably 200 μm, even more preferably 150 μm, even more preferably 100 μm, even more preferably 80 μm, even more preferably 70 μm, even more preferably 60 μm, even more preferably 50 μm, and the lower limit is more preferably 5 μm, even more preferably 10 μm, even more preferably 20 μm, even more preferably 30 μm.
[0128] The thickness of the electrically peelable pressure-sensitive adhesive sheet according to the embodiment of the present invention is preferably 20 μm or more and 3000 μm or less. The upper limit of the thickness is more preferably 1000 μm, even more preferably 500 μm, even more preferably 300 μm, even more preferably 250 μm, even more preferably 200 μm, even more preferably 150 μm, even more preferably 100 μm, and the lower limit is more preferably 30 μm, even more preferably 50 μm.
[0129] In particular, in the case of electrically peelable pressure-sensitive adhesive sheets X1 and X2 shown in Figures 1 and 2, the thickness of the electrically peelable pressure-sensitive adhesive sheet is preferably 20 μm or more and 2000 μm or less. The upper limit of the thickness is more preferably 1000 μm, even more preferably 500 μm, even more preferably 300 μm, even more preferably 250 μm, even more preferably 200 μm, even more preferably 150 μm, and the lower limit is more preferably 30 μm, even more preferably 50 μm, even more preferably 100 μm.
[0130] In particular, in the case of the electrically peelable pressure-sensitive adhesive sheet X3 shown in Fig. 3, the thickness of the electrically peelable pressure-sensitive adhesive sheet is preferably 50 µm or more and 3000 µm or less. The upper limit of the thickness is more preferably 1000 µm, and even more preferably 500 µm, and the lower limit is more preferably 50 µm, and even more preferably 100 µm, and even more preferably 200 µm.
[0131] The electrically releasing adhesive layer of the electrically releasing adhesive sheet according to an embodiment of the present invention, and the surface of the adhesive layer if any, may be protected by a release liner. Examples of release liners include, but are not limited to, release liners in which the surface of a substrate (liner substrate) such as paper or plastic film is silicone-treated, and release liners in which the surface of a substrate (liner substrate) such as paper or plastic film is laminated with a polyolefin resin. The thickness of the release liner is, but is not limited to, preferably 10 μm or more, more preferably 20 μm or more, even more preferably 30 μm or more, and preferably 100 μm or less, more preferably 80 μm or less, and even more preferably 50 μm or less.
[0132] [Method for Producing Electrically Peelable Pressure-Sensitive Adhesive Sheet] The electrically peelable pressure-sensitive adhesive sheet according to the embodiment of the present invention can be produced by a known or commonly used production method.
[0133] The conductive layer in the electrically peelable pressure-sensitive adhesive sheet according to the embodiment of the present invention can be formed by applying a conductive layer-forming composition, such as a conductive polymer or a conductive paste, to a supporting substrate and drying and / or curing the composition. The conductive layer-forming composition may be, for example, a composition obtained by dissolving and dispersing a conductive polymer as a resin component and additives in a solvent, or a conductive paste obtained by dissolving and dispersing a resin component, a conductive filler, and additives in a solvent.
[0134] The electrically releasing adhesive layer in the electrically releasing adhesive sheet according to an embodiment of the present invention can be formed by, for example, applying a solution of the adhesive composition according to an embodiment of the present invention, if necessary, in a solvent, onto a release liner, followed by drying and / or curing. When providing other adhesive layers, the other adhesive layers can be formed by, for example, applying a solution of the adhesive composition, if necessary, in a solvent, onto a release liner, followed by drying and / or curing. The solvents and release liners listed above can be used.
[0135] For application, a conventional coater (for example, a gravure roll coater, a reverse roll coater, a kiss roll coater, a dip roll coater, a bar coater, a knife coater, a spray roll coater, etc.) can be used.
[0136] The above-mentioned method can be used to produce a conductive layer, an electrically peeling pressure-sensitive adhesive layer, and other pressure-sensitive adhesive layers, and by appropriately laminating a conductive substrate comprising a support substrate and a conductive layer, an electrically peeling pressure-sensitive adhesive layer, and, if necessary, other pressure-sensitive adhesive layers, an electrically peeling pressure-sensitive adhesive sheet according to an embodiment of the present invention can be produced.
[0137] [Method for Electrically Peeling Electrically Peelable Pressure-Sensitive Adhesive Sheet] Peeling of the electrically peelable pressure-sensitive adhesive sheet according to an embodiment of the present invention from an adherend can be achieved by applying a voltage to the electrically peelable pressure-sensitive adhesive layer, thereby generating a potential difference in the thickness direction of the electrically peelable pressure-sensitive adhesive layer. For example, an assembly in which electrically peelable pressure-sensitive adhesive sheet X1 or X2 is attached to a conductive adherend can be peeled by passing a current between the conductive layer and the conductive adherend and applying a voltage to the electrically peelable pressure-sensitive adhesive layer. For example, in the case of electrically peelable pressure-sensitive adhesive sheet X3, it can be peeled from the adherend by passing a current through both conductive layers and applying a voltage to the electrically peelable pressure-sensitive adhesive layer. The current is preferably applied by connecting terminals to one end and the other end of the electrically peelable pressure-sensitive adhesive sheet so that a voltage is applied to the entire electrically peelable pressure-sensitive adhesive layer. Note that, if the adherend has a metal surface, the one end and the other end may be part of the adherend having a metal surface. Note that, during peeling, water may be added to the interface between the adherend surface of the conductive adherend and the electrically peelable pressure-sensitive adhesive layer before applying a voltage.
[0138] [Uses of Electrically Releaseable Pressure-Sensitive Adhesive Sheets] Conventional re-peeling technologies include adhesive layers that are cured and peeled by ultraviolet (UV) irradiation, and adhesive layers that peel off by heat. Electrically releaseable pressure-sensitive adhesive sheets using such adhesive layers cannot be used in cases where ultraviolet (UV) irradiation is difficult or where heat damages the adherend. The electrically releaseable pressure-sensitive adhesive sheet according to an embodiment of the present invention, which includes the electrically releaseable pressure-sensitive adhesive layer, does not use ultraviolet or heat, and therefore can be easily peeled off by applying a voltage without damaging the adherend. Therefore, the electrically releaseable pressure-sensitive adhesive sheet according to an embodiment of the present invention is suitable for use in fixing secondary batteries (e.g., lithium-ion battery packs) used in mobile devices such as smartphones, mobile phones, laptops, video cameras, and digital cameras to the housings.
[0139] In addition, examples of rigid members that can be bonded with the electrically peelable pressure-sensitive adhesive sheet according to the embodiment of the present invention include silicon substrates for semiconductor wafers, sapphire substrates for LEDs, SiC substrates and metal-based substrates, TFT substrates and color filter substrates for displays, and base substrates for organic EL panels. Examples of fragile members that can be bonded with the double-sided electrically peelable pressure-sensitive adhesive sheet include semiconductor substrates such as compound semiconductor substrates, silicon substrates for MEMS devices, passive matrix substrates, surface cover glass for smartphones, OGS (One Glass Solution) substrates in which a touch panel sensor is attached to the cover glass, organic substrates and organic-inorganic hybrid substrates mainly composed of silsesquioxane, flexible glass substrates for flexible displays, and graphene sheets.
[0140] [Joint] The joined structure according to an embodiment of the present invention comprises an electrically peelable pressure-sensitive adhesive sheet according to an embodiment of the present invention and a conductive material, in which the electrically peelable pressure-sensitive adhesive layer of the electrically peelable pressure-sensitive adhesive sheet is adhered to the conductive material. The conductive material is preferably an adherend having a metal adhesion surface. Examples of adherends having a metal adhesion surface include those made of a metal primarily composed of aluminum, copper, iron, magnesium, tin, gold, silver, lead, etc., and among these, metals containing aluminum are preferred.
[0141] Examples of the bonded body according to the embodiment of the present invention include an electrically peelable pressure-sensitive adhesive sheet X1 and a bonded body in which the electrically peelable pressure-sensitive adhesive layer 1 side of the electrically peelable pressure-sensitive adhesive sheet X1 is attached to a conductive adherend having, for example, a metal adherend surface.
[0142]
[0023] In the case where the electrically releasing pressure-sensitive adhesive sheet according to an embodiment of the present invention further comprises another pressure-sensitive adhesive layer, a second conductive substrate containing a resin component, and a second other pressure-sensitive adhesive layer, the other pressure-sensitive adhesive layer being formed on the surface of the support substrate opposite the conductive layer, the second conductive substrate and the second other pressure-sensitive adhesive layer being formed in this order on the surface of the electrically releasing pressure-sensitive adhesive layer opposite the conductive layer, and the electrically releasing pressure-sensitive adhesive layer and the second conductive substrate being in contact with each other, another aspect of the joined body according to an embodiment of the present invention is a joined body comprising the electrically releasing pressure-sensitive adhesive sheet according to an embodiment of the present invention and an adherend material, and the other pressure-sensitive adhesive layer being attached to the adherend material. The adherend material is selected from conductive materials and non-conductive materials.
[0143] Examples of the bonded body according to the embodiment of the present invention include a bonded body in which the other adhesive layers 6 on both sides of the electrically peeling adhesive sheet X3 are adhered to a conductive material having, for example, a metal coating surface, and a bonded body in which any of the other adhesive layers 6 in the electrically peeling adhesive sheet X3 are adhered to a non-conductive material.
[0144] As described above, the present specification discloses the following: [1] An electrically releasing pressure-sensitive adhesive sheet comprising: a conductive substrate including a support substrate and a conductive layer containing a resin component; and an electrically releasing pressure-sensitive adhesive layer whose adhesive strength decreases upon application of a voltage, the electrically releasing pressure-sensitive adhesive layer being in contact with the conductive layer. [2] The electrically releasing pressure-sensitive adhesive sheet according to [1], wherein the electrically releasing pressure-sensitive adhesive layer contains a polymer and an ionic liquid. [3] The electrically releasing pressure-sensitive adhesive sheet according to [2], wherein the anion of the ionic liquid is at least one selected from the group consisting of bis(fluorosulfonyl)imide anion and bis(trifluoromethanesulfonyl)imide anion. [4] The electrically releasing pressure-sensitive adhesive sheet according to [2] or [3], wherein the cation of the ionic liquid is at least one selected from the group consisting of nitrogen-containing onium cations, sulfur-containing onium cations, and phosphorus-containing onium cations. [5] The electrically releasing pressure-sensitive adhesive sheet according to any one of [1] to [4], wherein the conductive layer contains a conductive polymer. [6] The electrically peelable pressure-sensitive adhesive sheet of [5], wherein the conductive polymer comprises at least one selected from PEDOT / PSS, a polyacetylene-based polymer, a polyaniline-based polymer, and a polypyrrole-based polymer. [7] The electrically peelable pressure-sensitive adhesive sheet of any one of [1] to [6], wherein the conductive layer further comprises a conductive filler. [8] The electrically peelable pressure-sensitive adhesive sheet of [7], wherein the conductive filler is carbon particles or metal particles. [9] The electrically peelable pressure-sensitive adhesive sheet of any one of [1] to [8], wherein the conductive layer has a surface resistance of 5000 Ω / □ or less.
[10] The electrically peelable pressure-sensitive adhesive sheet of any one of [1] to [9], further comprising another pressure-sensitive adhesive layer, the other pressure-sensitive adhesive layer being formed on the surface of the support substrate opposite to the conductive layer.
[11] The electrically releasing pressure-sensitive adhesive sheet according to any one of [1] to
[10] , further comprising another pressure-sensitive adhesive layer, a second conductive layer containing a resin component, and a second other pressure-sensitive adhesive layer, wherein the other pressure-sensitive adhesive layer is formed on the surface of the supporting substrate opposite the conductive layer, and the second conductive layer and the second other pressure-sensitive adhesive layer are formed in this order on the surface of the electrically releasing pressure-sensitive adhesive layer opposite the conductive layer, and the electrically releasing pressure-sensitive adhesive layer and the second conductive layer are in contact with each other.
[12] A bonded body comprising the electrically releasing pressure-sensitive adhesive sheet according to any one of [1] to
[11] and a conductive material, wherein the electrically releasing pressure-sensitive adhesive layer is adhered to the conductive material.
[13] A bonded body comprising the electrically releasing pressure-sensitive adhesive sheet according to
[12] and an adherend material, wherein the other pressure-sensitive adhesive layer is adhered to the adherend material.
[0145] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The weight average molecular weights shown below were measured by gel permeation chromatography (GPC) using the method described above.
[0146] (Preparation of Acrylic Polymer Solution) As monomer components, 87 parts by mass of n-butyl acrylate (BA), 10 parts by mass of 2-methoxyethyl acrylate (MEA), 3 parts by mass of acrylic acid (AA), and 150 parts by mass of ethyl acetate as a polymerization solvent were placed in a separable flask and stirred for 1 hour while introducing nitrogen gas. After removing oxygen from the polymerization system in this way, 0.2 parts by mass of 2,2'-azobisisobutyronitrile (AIBN) was added as a polymerization initiator, and the mixture was heated to 63°C and reacted for 6 hours. Thereafter, ethyl acetate was added to obtain an acrylic polymer solution with a solids concentration of 30% by mass. The weight average molecular weight of the obtained acrylic polymer 1 was 700,000.
[0147] [Examples 1 and 2] (Preparation of electrically peelable pressure-sensitive adhesive layer) The acrylic polymer (solution), crosslinking agent, ionic liquid, additives (adsorption inhibitor, chelating-type metal deactivator), and ethyl acetate obtained above were added and stirred and mixed to obtain each electrically peelable pressure-sensitive adhesive composition (solution) adjusted to a solids concentration of 25% by mass. The solids concentration of the electrically peelable pressure-sensitive adhesive composition refers to the mass ratio of all components other than the solvent to the total mass of the electrically peelable pressure-sensitive adhesive composition.
[0148] Table 1 shows the blending amount of each component. The value for each component in Table 1 below means parts by mass. The obtained electrically peelable pressure-sensitive adhesive composition (solution) was applied to a uniform thickness using an applicator onto the release-treated surface of a polyethylene terephthalate release liner (trade name "MRF38", manufactured by Mitsubishi Plastics, Inc.). The resulting composition was then dried by heating at 150°C for 3 minutes, and the release-treated surface of a polyethylene terephthalate release liner (trade name "MRE38", manufactured by Mitsubishi Plastics, Inc.) was then laminated onto the pressure-sensitive adhesive using a hand roller to obtain an electrically peelable pressure-sensitive adhesive layer having a thickness of 50 μm.
[0149] The abbreviations for the ionic liquid, crosslinking agent, adsorptive inhibitor, and chelating-type metal deactivator in Table 1 are as follows:
[0150] (Ionic liquid) AS-110: cation: 1-ethyl-3-methylimidazolium cation, anion: bis(fluorosulfonyl)imide anion, trade name "ELEXEL AS-110", manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd. (Crosslinking agent) V-05: polycarbodiimide resin, trade name "CARBODILITE V-05", manufactured by Nisshinbo Chemical Inc. (Adsorption inhibitor) AMINE O: 2-(8-heptadecen-1-yl)-4,5-dihydro-1H-imidazole-1-ethanol, trade name "AMINE O", manufactured by BASF Japan Ltd. Irgacor DSSG: sodium sebacate, trade name "Irgacor DSSG", manufactured by BASF Japan Ltd. (Chelate-forming metal deactivator) Irgamet 30: N,N-bis(2-ethylhexyl)-[(1,2,4-triazol-1-yl)methyl]amine, trade name "Irgamet 30", manufactured by BASF Japan Ltd.
[0151] (Preparation of three-layer electrically peeling double-sided pressure-sensitive adhesive sheet) The polyethylene terephthalate release liner (MRE38) was peeled off from each electrically peeling pressure-sensitive adhesive layer (adhesive sheet) prepared in the same manner as above, and the surface of the exposed electrically peeling pressure-sensitive adhesive layer was bonded to the conductive layer side of a conductive layer-attached film (conductive substrate) (product name "Staclear-NCF", manufactured by Nagaoka Sangyo Co., Ltd., film thickness approximately 100 μm, conductive layer thickness 350 nm, or product name "Daiclear DC-75", manufactured by Dainippon Packaging Co., Ltd., film thickness approximately 100 μm, conductive layer thickness 550 nm), which is a laminate comprising a conductive layer (conductive polymer layer / PEDOT-PSS) and a supporting substrate laminated in this order, to prepare a single-sided electrically peeling pressure-sensitive adhesive sheet. Furthermore, a double-sided tape (product name "No. 56405", manufactured by Nitto) was attached to the surface of the single-sided electrically peeling adhesive sheet facing the support substrate, to form a three-layer electrically peeling double-sided adhesive sheet in which one surface was an electrically peeling adhesive layer and the other surface was another adhesive layer.
[0152] (Production of bonded structure) The release liner (MRF38) was peeled off from the three-layer electrically peeling double-sided PSA sheet obtained above, and a stainless steel plate (SUS316, size: 30 mm × 120 mm) was attached as a conductive adherend to the peeled surface such that one end of the double-sided PSA sheet protruded from the adherend by approximately 20 mm, and the sheet was pressed back and forth once with a 2 kg roller and left to stand in an environment of 23°C for 30 minutes, thereby obtaining bonded structures of Examples 1 and 2 in which the electrically peeling pressure-sensitive adhesive layer 1 of the electrically peeling pressure-sensitive adhesive sheet was attached to the conductive adherend (conductive adherend 7 in Figure 4 ).
[0153] [Example 3] (Preparation of conductive substrate) To 100 parts by mass of a urethane resin (polyester urethane resin, UR-3210, manufactured by Toyobo Co., Ltd.), 180 parts by mass of carbon black (Denka Black, average particle size 35 nm, manufactured by Denka Co., Ltd.), 7 parts by mass of blocked isocyanate (BI-7960, manufactured by Baxenden Co., Ltd.), 3 parts by mass of a catalyst (KS-1260, manufactured by Kyodo Pharmaceutical Co., Ltd.), and 400 parts by mass of a solvent (isophorone) were added, and the mixture was stirred and degassed at room temperature to obtain a conductive paste. The obtained conductive paste was coated on a support substrate (50 μm, PET film, manufactured by Toray Industries, Inc.) with a wire bar and dried at 100 ° C. for 1 hour to form a conductive layer having a thickness of 8 μm on the PET film, thereby obtaining a conductive substrate of Example 3.
[0154] (Preparation of three-layer electrically peeling double-sided pressure-sensitive adhesive sheet and assembly) An electrically peeling pressure-sensitive adhesive layer was prepared in the same manner as above using an electrically peeling pressure-sensitive adhesive composition (solution, solids concentration 25% by mass) having the composition shown in Table 1, and a single-sided electrically peeling pressure-sensitive adhesive sheet, a three-layer electrically peeling double-sided pressure-sensitive adhesive sheet and an assembly of Example 3 were prepared in the same manner as Example 1, except that the conductive substrate used in Example 1 was changed to the conductive substrate obtained above.
[0155] [Examples 4 and 5] Conductive substrates, three-layer electrically peelable double-sided sheets, and bonded bodies of Examples 4 and 5 were prepared in the same manner as in Example 1, except that the thickness of the conductive layer was set to 3 μm and 2 μm, respectively.
[0156] [Example 6] (Preparation of conductive substrate) To 100 parts by mass of a urethane resin (polyester urethane resin, UR-3210, manufactured by Toyobo Co., Ltd.), 80 parts by mass of silver powder (FA-2-3, average particle size 5 μm, manufactured by Dowa Mining Co., Ltd.), 7 parts by mass of blocked isocyanate (BI-7960, manufactured by Baxenden Co., Ltd.), 3 parts by mass of a catalyst (KS-1260, manufactured by Kyodo Pharmaceutical Co., Ltd.), and 400 parts by mass of a solvent (isophorone) were added, stirred at room temperature, and degassed to obtain a conductive paste. The obtained conductive paste was coated on a support substrate (50 μm, PET film, manufactured by Toray Industries, Inc.) with a wire bar and dried at 100 ° C. for 1 hour to form a conductive layer having a thickness of 1 μm on the PET film, thereby obtaining a conductive substrate of Example 6.
[0157] (Preparation of three-layer electrically peeling double-sided pressure-sensitive adhesive sheet and assembly) An electrically peeling pressure-sensitive adhesive layer was prepared in the same manner as above using an electrically peeling pressure-sensitive adhesive composition (solution, solids concentration 25% by mass) having the composition shown in Table 1, and a single-sided electrically peeling pressure-sensitive adhesive sheet, a three-layer electrically peeling double-sided pressure-sensitive adhesive sheet and an assembly of Example 6 were prepared in the same manner as Example 1, except that the conductive substrate used in Example 1 was changed to the conductive substrate obtained above.
[0158] Comparative Example 1 An electrically peeling pressure-sensitive adhesive layer was prepared in the same manner as above using an electrically peeling pressure-sensitive adhesive composition (solution, solids concentration 25% by mass) having the composition shown in Table 1, and the conductive substrate was changed to a metal layer-attached film (product name "Metal Me TS", manufactured by Toray Industries, Inc., thickness 50 μm), which is a laminate comprising an electrically conductive layer (metal layer) and a support substrate laminated in this order, and the metal layer side of the metal layer-attached film was attached to the exposed surface of the electrically peeling pressure-sensitive adhesive layer. In the same manner as in Examples 1 and 2, except for this, a single-sided electrically peeling pressure-sensitive adhesive sheet, a three-layer electrically peeling double-sided pressure-sensitive adhesive sheet and an assembly of Comparative Example 1 were obtained.
[0159] Comparative Example 2 An electrically peeling pressure-sensitive adhesive layer was prepared in the same manner as above using an electrically peeling pressure-sensitive adhesive composition (solution, solids concentration 25% by mass) having the composition shown in Table 1, and the conductive substrate was changed to a metal layer-attached film (product name "1005CR", manufactured by Toray Advanced Film Co., Ltd., thickness 12 μm) which is a laminate comprising a coating layer, a conductive layer (metal layer), and a support substrate laminated in this order, and the coating layer side of the metal layer-attached film was attached to the exposed surface of the electrically peeling pressure-sensitive adhesive layer, and the same procedures were carried out as in Examples 1 and 2, except that a single-sided electrically peeling pressure-sensitive adhesive sheet, a three-layer electrically peeling double-sided pressure-sensitive adhesive sheet, and an assembly of Comparative Example 2 were obtained.
[0160] Comparative Example 3 An electrically peeling pressure-sensitive adhesive layer was prepared in the same manner as above using an electrically peeling pressure-sensitive adhesive composition (solution, solids concentration 25% by mass) having the composition shown in Table 1, and the conductive substrate was changed to a metal layer-attached film (product name "DMS(X42)PC", manufactured by Toray Advanced Film Co., Ltd., thickness 50 μm) which is a laminate comprising a coating layer, a conductive layer (metal layer), and a supporting substrate laminated in this order, and the coating layer side of the metal layer-attached film was attached to the exposed surface of the electrically peeling pressure-sensitive adhesive layer, and the same procedures were carried out as in Examples 1 and 2, except that a single-sided electrically peeling pressure-sensitive adhesive sheet, a three-layer electrically peeling double-sided pressure-sensitive adhesive sheet, and an assembly of Comparative Example 3 were obtained.
[0161] (Initial Adhesion Strength (22°C / 50% RH 72 hr)) Evaluation was carried out for Examples 1 to 6 and Comparative Examples 1 to 3. The produced bonded structures were allowed to stand at 22°C and 50% RH for 72 hours, and then peeled in the direction of the arrow in Fig. 4 using a peel tester (product name "Variable Angle Peel Tester YSP", manufactured by Asahi Seiko Co., Ltd.), and the adhesive strength (22°C / 50% RH 72 hr) in a 180° peel test (tensile speed: 300 mm / min, peel temperature: 23°C) was measured.
[0162] (Initial Adhesion Strength (60°C / 90% RH 600 hr)) The above bonded body was stored in a thermo-hygrostat at 60°C / 90% RH for 600 hours, and after being taken out, was left to stand at 22°C / 50% RH for 30 minutes to cool down. Thereafter, the adhesive strength (60°C / 90% RH 600 hr) was measured in the same manner as in the above adhesive strength measurement.
[0163] (Electric Peeling Force (22°C / 50% RH 72 hr)) Prior to peeling, positive and negative electrodes of a DC current machine were attached to the positions α and β of the bonded body in Figure 4, respectively, and a voltage of 50 V was applied for 60 seconds. After that, the bonded body was peeled in the direction of the arrow in Figure 4. In the same manner as in the above-mentioned measurement of adhesive strength, the electric peeling force (22°C / 50% RH 72 hr) was measured.
[0164] (Electrical Peel Force (60°C / 90% RH 600 hr)) The bonded body was stored in a thermo-hygrostat at 60°C / 90% RH for 600 hours, and after removal, was left to stand at 22°C / 50% RH for 30 minutes to cool. Thereafter, the electrical peel force (60°C / 90% RH 600 hr) was measured in the same manner as in the electrical peel force measurement described above.
[0165] When measuring the initial adhesive strength and electrical peel strength, the surface of the adherend was checked after peeling. When vapor deposition peeling occurred, with the electrically peeling pressure-sensitive adhesive layer and the metal layer peeling from the support substrate remaining on the adherend surface, it was rated as "vapor deposition peeling," when the electrically peeling pressure-sensitive adhesive layer separated from the support substrate and transferred to the adherend surface, it was rated as "anchoring failure," and when the metal layer corroded and the electrically peeling pressure-sensitive adhesive layer separated only at the corroded points and transferred to the adherend surface, it was rated as "corroded anchor failure."
[0166] (Surface Resistance of Conductive Layer) The surface resistance of the conductive layer was measured on the surface of the conductive substrate on the conductive layer side using the conductive substrate used in Examples 1 to 6 and Comparative Examples 1 to 3 as test samples, using Loresta GP (MCP-T160) manufactured by Mitsubishi Chemical Analytech Co., Ltd. under conditions of an applied voltage of 10 V and an application time of 10 seconds. The surface resistance was measured in an environment of a temperature of 25°C ± 5°C and a relative humidity of 50 ± 5%.
[0167] The results obtained are shown in Table 1.
[0168]
[0169] The results in Table 1 show that the electrically peelable pressure-sensitive adhesive sheets of the Examples can suppress peeling of the conductive layer from the support substrate and the electrically peelable pressure-sensitive adhesive layer from the conductive layer, even when placed in a high-temperature, high-humidity environment for a long period of time, and can maintain sufficient adhesive strength. Furthermore, it was found that the adhesive strength is sufficiently reduced by the application of voltage, and the sheets exhibit the functionality required for an electrically peelable pressure-sensitive adhesive sheet.
[0170] On the other hand, in Comparative Examples 1 to 3, when the electrically releasing pressure-sensitive adhesive sheet was placed in a high-temperature, high-humidity environment for a long period of time, the electrically releasing pressure-sensitive adhesive layer separated from the supporting substrate when an attempt was made to peel the sheet from the adherend. In Comparative Example 3, the electrically releasing pressure-sensitive adhesive layer separated from the electrically releasing pressure-sensitive adhesive sheet only at the corroded areas of the metal layer. In other words, it was shown that the sheets of Comparative Examples 1 to 3 could not be peeled at the intended interface and did not function as electrically releasing pressure-sensitive adhesive sheets.
[0171] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention.
[0172] The electrically peelable pressure-sensitive adhesive sheet of the present invention can suppress peeling of the conductive layer from the support substrate due to application of voltage, and can suppress peeling of the electrically peelable pressure-sensitive adhesive layer from the conductive layer, even when stored in a high-temperature, high-humidity environment for a long period of time, thereby maintaining sufficient adhesive strength.
[0173] Although the present invention has been described in detail and with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on Japanese patent applications filed on March 29, 2023 (Patent Application No. 2023-54108) and January 31, 2024 (Patent Application No. 2024-13137), the contents of which are incorporated herein by reference.
[0174] X1, X2, X3 Electrically peelable pressure-sensitive adhesive sheet 1 Electrically peelable pressure-sensitive adhesive layer 3 Conductive layer 4 Support substrate 5 Conductive substrate 6 Other pressure-sensitive adhesive layer 7 Conductive adherend 8 Laminate
Claims
1. An electrically peelable adhesive sheet comprising: a conductive substrate including a supporting substrate and a conductive layer containing a resin component; and an electrically peelable adhesive layer the adhesive strength of which decreases upon application of a voltage, the electrically peelable adhesive layer being in contact with the conductive layer.
2. The electrically peelable adhesive sheet according to claim 1, wherein the electrically peelable adhesive layer contains a polymer and an ionic liquid.
3. The electrically peelable pressure-sensitive adhesive sheet according to claim 2, wherein the anion of the ionic liquid is at least one selected from the group consisting of bis(fluorosulfonyl)imide anion and bis(trifluoromethanesulfonyl)imide anion.
4. The electrically peelable adhesive sheet according to claim 2, wherein the cation of the ionic liquid is at least one selected from the group consisting of nitrogen-containing onium cations, sulfur-containing onium cations, and phosphorus-containing onium cations.
5. The electrically peelable pressure-sensitive adhesive sheet according to claim 1 or 2, wherein the conductive layer comprises a conductive polymer.
6. The electrically peelable pressure-sensitive adhesive sheet according to claim 5, wherein the conductive polymer comprises at least one selected from the group consisting of PEDOT / PSS, polyacetylene-based polymers, polyaniline-based polymers, and polypyrrole-based polymers.
7. The electrically peelable pressure-sensitive adhesive sheet according to claim 1 or 2, wherein the conductive layer further comprises a conductive filler.
8. The electrically peelable pressure-sensitive adhesive sheet according to claim 7, wherein the conductive filler is carbon particles or metal particles.
9. The electrically peelable pressure-sensitive adhesive sheet according to claim 1 or 2, wherein the surface resistance of the conductive layer is 5000 Ω / □ or less.
10. An electrically peelable adhesive sheet as described in claim 1 or 2, further comprising another adhesive layer, said another adhesive layer being formed on the surface of said supporting substrate opposite said conductive layer.
11. An electrically peelable adhesive sheet as described in claim 1 or 2, further comprising another adhesive layer, a second conductive layer containing a resin component, and a second other adhesive layer, wherein the other adhesive layer is formed on the surface of the supporting substrate opposite the conductive layer, the second conductive layer and the second other adhesive layer are formed in this order on the surface of the electrically peelable adhesive layer opposite the conductive layer, and the electrically peelable adhesive layer and the second conductive layer are in contact with each other.
12. An assembly comprising the electrically peelable adhesive sheet according to claim 1 or 2 and a conductive material, wherein the electrically peelable adhesive layer is attached to the conductive material.
13. A joint comprising the electrically peelable adhesive sheet according to claim 11 and an adherend material, with the other adhesive layer being attached to the adherend material.
Citation Information
Patent Citations
electrical decoupling substance
JP2003504504A
Electrically peelable pressure-sensitive adhesive article and method for peeling off the same
JP2011052056A
Electrically peelable composition for high temperature exposure
WO2021202527A1
Electrically peelable adhesive sheet and bonded body
WO2022030565A1
Adhesive composition for electical peeling, adhesive sheet and bonded body
WO2022163593A1
Cited By
Device capable of bonding and debonding on demand
WO2026099153A1
Device capable of stain-free debonding on demand
WO2026099181A1
Anti-corrosion adhesive device
WO2026099184A1
Double-sided pressure-sensitive adhesive sheet, joined body, electrical / electronic appliance, and method for producing pressure-sensitive adhesive sheet
WO2026155040A1
Laminate, primer layer, joined body, and method for manufacturing joined body
WO2026197437A1