Material for three-dimensional modeling, molded body and method for producing same

The combination of resin powders with specific particle size distributions in three-dimensional modeling materials addresses the issue of poor mechanical properties in powder bed fusion, resulting in improved impact resistance and formability for practical applications.

WO2024204368A1PCT designated stage expired Publication Date: 2024-10-03MITSUBISHI CHEM CORP

Patent Information

Application Number
PCT/JP2024/012279
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Three-dimensional printing using the powder bed fusion method often results in molded products with poor mechanical properties and low impact resistance, making them unsuitable for practical applications such as home appliances, building materials, and automotive components, due to the formation of voids and inadequate material properties.

Method used

A three-dimensional modeling material comprising two types of resin powders with different compositions and particle sizes, where one resin powder has an average particle diameter of 30 μm to 250 μm and the other has a smaller average particle size of 1 μm to 30 μm, with specific particle size distribution characteristics, enhancing the mechanical strength and impact resistance of the molded products.

Benefits of technology

The use of this material improves the formability and impact resistance of the printed objects, making them suitable for functional parts in practical applications by reducing voids and enhancing mechanical strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure 00000040_0000
    Figure 00000040_0000
  • Figure 00000040_0001
    Figure 00000040_0001
Patent Text Reader

Abstract

Provided is a three-dimensional modeling material that contains a resin powder (A) having an average particle size (D50) by a laser diffraction method of 30-250 μm inclusive and a resin powder (B) that is a resin composition different from the resin powder (A) and has an average particle size (D50) by a laser diffraction method of from 1 μm to less than 30 μm. Provided is a three-dimensional modeling material that contains a resin powder (A) having an average particle size (D50) by a laser diffraction method of 30-250 μm and a resin powder (B) that is a resin composition different from the resin powder (A) and has an average particle size (D50) by a laser diffraction method of 3-30% inclusive of the average particle size (D50) of the resin powder (A). Provided is a three-dimensional modeling material that contains a resin powder (A) that has a plurality of peaks between 5 μm and 250 μm in a number-based particle size distribution chart obtained by image analysis and has a peak top on the largest particle size side of the plurality of peaks and a resin powder (B) that has a peak top 20 μm or less below the peak top of the resin powder (A).
Need to check novelty before this filing date? Find Prior Art

Description

Three-dimensional modeling material, molded body, and method for manufacturing the same

[0001] The present invention relates to a material for three-dimensional modeling, more particularly to a material for three-dimensional modeling containing two types of resin powder having different resin compositions and particle sizes. The present invention also relates to a molded product using this material for three-dimensional modeling and a method for producing the same.

[0002] Today, three-dimensional printers (hereinafter sometimes referred to as "3D printers") using various additive manufacturing methods (e.g., binder jetting, material extrusion, liquid vat photopolymerization, etc.) are commercially available. Among these, 3D printer systems using the Powder Bed Fusion method, such as the system manufactured by 3D Systems, Inc. in the United States, fuse a thin layer (powder bed) of powder material such as resin using a high-power CO 2 This method uses a heating means such as a laser to heat and melt the resin powder to a temperature near its melting point, allowing for the layered construction of a three-dimensional object based on a computer-aided design (CAD) model. The laser used as the heating means selectively melts the powder material by scanning the cross section in the X-Y direction across the surface of a powder bed formed based on 3D CAD data. In this way, a three-dimensional molded object can be obtained by repeatedly forming a powder bed and fusing it with a laser to form a layered structure. This system does not require the use of molds, can use a variety of resin powders as raw materials as long as they have a certain degree of heat resistance, and produces highly reliable molded objects. This technology has attracted attention in recent years.

[0003] Crystalline thermoplastic resins are used as the resin powder material for 3D printers due to their molding principles. Polyamide resins such as nylon 12 and nylon 11 are particularly widely used. In recent years, polyester resins such as polybutylene terephthalate, polyolefin resins such as polypropylene, and elastomer resins such as thermoplastic polyurethane have also come into use.

[0004] Traditionally, 3D printers have been widely used for product prototyping. In recent years, the application of 3D printers to functional parts for practical use has also been considered. When considering practical use, for example, as components for home appliances, building materials, aircraft, automotive materials, etc., it is desirable that the molded articles obtained using 3D printers using 3D modeling materials have high mechanical properties.

[0005] However, due to the manufacturing principle, compacts produced by the Powder Bed Fusion method are prone to voids within the compact, resulting in poor mechanical properties. In particular, it is difficult to impart high impact resistance to the materials currently used in automotive components.

[0006] For example, the following proposals have been made to improve the mechanical properties of molded bodies produced by the Powder Bed Fusion method. Patent Document 1 discloses a method for obtaining powder with excellent tensile elongation at break by specifying the ethylene molar ratio and melt flow rate of a polypropylene resin within specific ranges. Patent Document 2 discloses a method for obtaining powder with excellent strength in the lamination direction of a molded body by melt-kneading talc as a filler with a polypropylene resin and specifying the mass ratio of silicon oxide to the total mass of the obtained resin powder within a specific range.

[0007] International Publication No. 2020 / 213586 Japanese Patent Application Laid-Open No. 2020-93515

[0008] In order for 3D printers to be widely applied to functional parts that are also used in practical applications, it is desirable to be able to use existing resin powders to improve the shaping properties of 3D printers and the impact resistance of the resulting molded bodies, as well as to ensure safety during material production.

[0009] However, Patent Document 1 requires the polymerization of an ethylene-propylene copolymer with a specific composition, which is undesirable from the viewpoint of the production and procurement of raw materials. Patent Document 2 contains talc that falls under the GHS classification, which raises safety concerns during pulverization. In both examples, improvement in the impact resistance of the resulting molded body has not been confirmed.

[0010] The present invention aims to provide a three-dimensional modeling material containing a resin composition, which uses existing resin powders, and which has excellent modeling properties in a 3D printer and excellent impact resistance of the resulting molded body while maintaining safety during powder production.

[0011] The inventors discovered that these problems can be solved by using two types of resin powders that differ in resin composition and particle size, or by using a three-dimensional modeling material that contains two types of resin powders that have different peak tops in a particle size distribution chart obtained by image analysis, and developed the present invention.

[0012] The gist of the present invention is as follows.

[0013] [1] A material for three-dimensional modeling, comprising: a resin powder (A) having an average particle size (D50) measured by a laser diffraction method of 30 μm or more and 250 μm or less; and a resin powder (B) having a resin composition different from that of the resin powder (A) and having an average particle size (D50) measured by a laser diffraction method of 1 μm or more and less than 30 μm.

[0014] [2] The material for three-dimensional modeling according to [1], wherein the average particle size (D50) of the resin powder (B) is 3% to 30% of the average particle size (D50) of the resin powder (A).

[0015] [3] A material for three-dimensional modeling, comprising: a resin powder (A) having an average particle size (D50) measured by a laser diffraction method of 30 μm or more and 250 μm or less; and a resin powder (B) having a resin composition different from that of the resin powder (A) and having an average particle size (D50) measured by a laser diffraction method of 3% or more and 30% or less of the average particle size (D50) of the resin powder (A).

[0016] [4] A material for three-dimensional modeling, characterized in that in a particle size distribution chart on a number basis obtained by image analysis using the following method, the material has multiple peaks between 5 μm and 250 μm, with at least one peak top in the region of 5 μm or more and smaller than 30 μm, and in a particle size distribution chart on a volume basis obtained by image analysis, the material has a peak top in the region of 5 μm or more and smaller than 30 μm, with the volume-based peak top value being 2.5 times or less the value of at least one number-based peak top, and the volume-based average particle size (D50) being 30 μm or more. Image analysis method: 1 cc of resin powder is spread on a slide and observed under the following observation conditions, and particle size analysis is performed under the following particle size analysis conditions. (Observation conditions) Measuring device: XploRA Plus manufactured by HORIBA, Ltd. Observation illumination: transmitted light Objective lens: Olympus bright / dark field plan achromat MPLN 10 xBD Observation field: 15 x 11 mm area (composite image of 17 x 15 fields of view) (Particle size analysis conditions) Particle size analysis software: Particle Finder ver. 2 Particle size cutoff: equivalent circle diameter of 4 μm or more Circularity cutoff: circularity of 0.6 or more Distribution criteria: number distribution and volume distribution

[0017] [5] The material for three-dimensional modeling according to any one of [1] to [4], wherein the resin powder (A) has an average particle size (D50) of 35 μm or more, 40 μm or more, 45 μm or more, or 50 μm or more. [6] The material for three-dimensional modeling according to any one of [1] to [5], wherein the resin powder (A) has an average particle size (D50) of 200 μm or less, 150 μm or less, or 120 μm or less. [7] The material for three-dimensional modeling according to any one of [1] to [6], wherein the resin powder (B) has an average particle size (D50) of 5% or more or 10% or more of that of the resin powder (A). [8] The material for three-dimensional modeling according to any one of [1] to [7], wherein the resin powder (B) has an average particle size (D50) of 25% or less or 20% or less of that of the resin powder (A).

[0018] [9] The material for three-dimensional modeling according to [4], wherein the resin powder (B) has a resin composition different from the resin powder (A).

[0019]

[10] The material for three-dimensional modeling according to [4] or [9], wherein the peak top of the resin powder (B) is 100 μm or less higher than the peak top of the resin powder (A).

[0020]

[11] The material for three-dimensional modeling according to any one of [1] to

[10] , wherein the resin powder (A) is a powder of a polyolefin resin.

[0021]

[12] The three-dimensional modeling material according to

[11] , wherein the polyolefin resin is a propylene polymer.

[0022]

[13] The three-dimensional modeling material according to any one of [1] to

[12] , wherein the resin powder (B) is a powder of at least one of polyethylene and a thermosetting elastomer.

[0023]

[14] The three-dimensional modeling material according to

[13] , wherein the polyethylene has a viscosity average molecular weight (Mv) of 500,000 or more and 10,000,000 or less.

[15] The three-dimensional modeling material according to

[13] or

[14] , wherein the polyethylene has a viscosity average molecular weight (Mv) of 1,000,000 or more or 2,000,000 or more.

[16] The three-dimensional modeling material according to any of

[13] to

[15] , wherein the polyethylene has a viscosity average molecular weight (Mv) of 6,000,000 or less or 3,000,000 or less.

[0024]

[17] The material for three-dimensional modeling according to any one of [1] to

[16] , wherein the content of the resin powder (B) is 1% by mass or more, 5% by mass or more, or 10% by mass or more relative to the total amount of the resin powder (A) and the resin powder (B).

[0025]

[18] The material for three-dimensional modeling according to any one of [1] to

[17] , wherein the content of the resin powder (B) is less than 50% by mass, 45% by mass or less, or 40% by mass or less, based on the total amount of the resin powder (A) and the resin powder (B).

[0026]

[19] The material for three-dimensional modeling according to any one of [1] to

[18] , which is in powder form.

[0027]

[20] The material for three-dimensional modeling according to any one of [1] to

[19] , which is a material for three-dimensional modeling by a powder bed fusion method.

[0028]

[21] A molded product obtained using the material for three-dimensional modeling according to any one of [1] to

[20] .

[0029]

[22] A method for manufacturing a molded body, comprising a step of three-dimensionally molding a molded body by a powder bed fusion method using the material for three-dimensional modeling according to any one of [1] to

[21] .

[0030] According to the present invention, it is possible to provide a material for three-dimensional modeling that uses existing resin powders, and that has excellent modeling properties in a 3D printer and excellent impact resistance of the resulting molded body while maintaining safety during powder production. Furthermore, according to the present invention, a molded body produced by powder bed fusion using this three-dimensional modeling material and a method for producing the same are provided.

[0031] 1 shows the particle size distribution on a number basis in Example 1. FIG. 2 shows the particle size distribution on a volume basis in Example 1. FIG. 3 shows the particle size distribution on a number basis in Example 2. FIG. 4 shows the particle size distribution on a volume basis in Example 2. FIG. 5 shows the particle size distribution on a number basis in Example 3. FIG. 6 shows the particle size distribution on a volume basis in Example 3. FIG. 7 shows the particle size distribution on a number basis in Example 4. FIG. 8 shows the particle size distribution on a volume basis in Example 4. FIG. 9 shows the particle size distribution on a number basis in Comparative Example 1. FIG. 10 shows the particle size distribution on a volume basis in Comparative Example 1. FIG. 11 shows the particle size distribution on a number basis in Comparative Example 2. FIG. 12 shows the particle size distribution on a volume basis in Comparative Example 2. FIG. 13 shows the particle size distribution on a number basis in Comparative Example 3. FIG. 14 shows the particle size distribution on a volume basis in Comparative Example 3.

[0032] Hereinafter, a mode for carrying out the present invention (hereinafter referred to as "the present embodiment") will be described in detail. The following present embodiment is an example for explaining the present invention, and is not intended to limit the present invention to the following content. The present invention can be carried out in various modified forms within the scope of its gist.

[0033] [Material for Three-Dimensional Modeling] The material for three-dimensional modeling of the present invention contains a resin powder (A) (hereinafter, may be referred to as "resin powder (A) of the present invention") and a resin powder (B) (hereinafter, may be referred to as "resin powder (B) of the present invention").

[0034] A three-dimensional modeling material according to a first embodiment of the present invention is characterized in that the resin powder (A) and the resin powder (B) have different resin compositions, and the resin powder (A) has an average particle size (D50) of 30 μm or more and 250 μm or less, as measured by a laser diffraction method, and the resin powder (B) has an average particle size (D50) of 1 μm or more and less than 30 μm, as measured by a laser diffraction method. In the first embodiment of the present invention, the average particle size (D50) of the resin powder (B) is preferably 3% or more and 30% or less of the average particle size (D50) of the resin powder (A).

[0035] A three-dimensional modeling material according to a second embodiment of the present invention is characterized in that the resin powder (A) and the resin powder (B) have different resin compositions, the resin powder (A) has an average particle size (D50) of 30 μm or more and 250 μm or less as measured by a laser diffraction method, and the resin powder (B) has an average particle size (D50) of 3% or more and 30% or less of the average particle size (D50) of the resin powder (A) as measured by a laser diffraction method.

[0036] A material for three-dimensional modeling according to a third embodiment of the present invention is characterized in that, in a particle size distribution chart on a number basis obtained by image analysis using the following method, it has multiple peaks between 5 μm and 250 μm and has at least one number-based peak top in a region of 5 μm or more and smaller than 30 μm, and in a particle size distribution chart on a volume basis obtained by image analysis, it has a volume-based peak top in a region of 5 μm or more and smaller than 30 μm, the value of the volume-based peak top being 2.5 times or less the value of at least one number-based peak top, and the volume-based average particle size (D50) is 30 μm or more. Image analysis method: 1 cc of resin powder is spread on a slide and observed under the following observation conditions, and particle size analysis is performed under the following particle size analysis conditions. (Observation conditions) Measuring device: XploRA Plus manufactured by HORIBA, Ltd. Observation illumination: transmitted light Objective lens: Olympus bright / dark field plan achromat MPLN 10 xBD Observation field: 15 x 11 mm area (composite image of 17 x 15 fields of view) (Particle size analysis conditions) Particle size analysis software: Particle Finder ver. 2 Particle size cutoff: equivalent circle diameter of 4 μm or more Circularity cutoff: circularity of 0.6 or more Distribution criteria: number distribution and volume distribution In the third embodiment of the present invention, it is preferable that the resin composition of the resin powder (A) and the resin composition of the resin powder (B) are different, and it is preferable that the peak top of the resin powder (B) is 100 μm or less higher than the peak top of the resin powder (A).

[0037] In this specification, the three-dimensional modeling material according to the first embodiment of the present invention, the three-dimensional modeling material according to the second embodiment of the present invention, and the three-dimensional modeling material according to the third embodiment of the present invention are collectively referred to as the “three-dimensional modeling material of the present invention.” In addition, the resin that is the material for resin powder (A) may be referred to as “resin (a),” and the resin that is the material for resin powder (B) may be referred to as “resin (b).”

[0038] The material for three-dimensional modeling of the present invention is used in a powder bed fusion method and contains at least the resin powder (A) and the resin powder (B) of the present invention.

[0039] The three-dimensional modeling material of the present invention is preferably a material used for forming a three-dimensional object (resin molded body) using a 3D printer, particularly using a Powder Bed Fusion method.

[0040] The shape of the material for three-dimensional modeling may be any shape that is applicable to various types of 3D printers, such as Powder Bed Fusion, Multi Jet Fusion, etc. The material for three-dimensional modeling of the present invention is preferably used for Powder Bed Fusion.

[0041] [Mechanism] Although the details of the mechanism by which the present invention achieves the above-described effects are not clear, it is presumed as follows.

[0042] That is, in both the first and second embodiments of the three-dimensional modeling materials of the present invention, the resin powder (A) and the resin powder (B) have different resin compositions, and the particle sizes of the resin powder (A) and the resin powder (B) are within a predetermined range, and the particle size of the resin powder (B) is smaller than the particle size of the resin powder (A). Therefore, the resin powder (B) is present between the particles of the resin powder (A) and is more likely to be included in the model layer produced by the melting and flowing of the resin powder (A).

[0043] Furthermore, the three-dimensional modeling material according to the third embodiment of the present invention has multiple peaks between 5 μm and 250 μm, and at least one number-based peak top in the region of 5 μm or more and smaller than 30 μm. In a volume-based particle size distribution chart obtained by image analysis, the material has a volume-based peak top in the region of 5 μm or more and smaller than 30 μm, and the value of the volume-based peak top is 2.5 times or less the value of at least one number-based peak top. Furthermore, the volume-based average particle size (D50) is 30 μm or more. This allows small particles to be present not only between large particles but also on the surfaces of the large particles. This makes it easier for the small particles to be included in the modeling layer produced by melting and flowing the large particles.

[0044] As a result, cracks and defects are less likely to occur in the molded body, the mechanical strength of the three-dimensional object can be improved, and it is thought that molded bodies with excellent impact resistance can be produced with excellent moldability.

[0045] [Definition of Physical Properties] The various physical properties in the present invention are values ​​measured as follows.

[0046] <Viscosity Average Molecular Weight (Mv)> The viscosity average molecular weight (Mv) of resin powder (A) and resin powder (B) is a value determined for resin powder (A) and resin powder (B) in accordance with the method specified in JIS K-736. However, in the case of ultra-high molecular weight polyethylene, it is a value calculated in accordance with the method specified in ASTM D4020, using the specific viscosity ηsp (dl / g) of a 0.05% decalin solution at 135°C instead of the intrinsic viscosity [η] (dl / g).

[0047] <Average particle size (D50)> The average particle size (D50) of the resin powder (A), the resin powder (B), and the powder of the material for three-dimensional modeling is determined by measuring the particle size distribution of the powder on a volume basis using a particle size distribution measuring device that uses a laser diffraction method, and determining the particle size at 50% of the frequency distribution of the powder within the detected particle size distribution.

[0048] <Peaks and Peak Tops in a Number-Based Particle Size Distribution Chart Obtained by Image Analysis> The peaks and peak tops in a number-based particle size distribution chart obtained by image analysis of the powder of the material for three-dimensional modeling according to the third embodiment of the present invention can be determined by observing the powder spread on a glass slide using a particle size distribution meter with an analysis function (for example, "XploRA PLUS" manufactured by HORIBA France SAS) equipped with particle size analysis software on a confocal laser Raman microscope, and creating a particle size distribution chart on a number-based basis using circle-equivalent diameters calculated from the areas of the obtained particle images.

[0049] <Melting Point (Tm) and Glass Transition Temperature (Tg)> The melting points (Tm) of the resin powders (A) and (B) are crystalline melting temperatures (melting points Tm) (°C) (reheating process) determined from thermograms measured using a differential scanning calorimeter in accordance with JIS K7121, in which the powders are heated from room temperature to 200°C at a heating rate of 10°C / min, held at that temperature for 1 minute, cooled to 50°C at a heating rate of 10°C / min, and then heated again to 200°C at a heating rate of 10°C / min. The glass transition temperatures (Tg) of the resin powders (A) and (B) are values ​​of glass transition temperature determined from thermograms measured using a differential scanning calorimeter in accordance with JIS K7121, in which the temperature was increased from room temperature to 200°C at a rate of 10°C / min, maintained at that temperature for 1 minute, then decreased to 50°C at a rate of 10°C / min, and then increased again to 200°C at a rate of 10°C / min.

[0050] <Resin Composition> In the present invention, "different resin compositions" means that, among the structural units (monomer species of resin raw materials) constituting the resin, the structural units that constitute the main component (structural units contained in the resin at 50% by mass or more) are different. Therefore, for example, propylene-based copolymers that differ in structural units other than propylene units are considered to have the same resin composition.

[0051] In the present invention, the "different resin compositions" can be confirmed by a microscopic IR method or a microscopic Raman spectroscopy.

[0052] [Resin Powder] The resin powders used in the three-dimensional modeling material of the present invention, i.e., resin powder (A) and resin powder (B), particularly resin powder (A), are preferably obtained using a thermoplastic resin. The resin powder may contain other resins other than the thermoplastic resin, additives, reinforcing materials, etc., to the extent that the effects of the present invention are not impaired. Alternatively, commercially available three-dimensional modeling materials made of thermoplastic resins may be used as the resin powder.

[0053] <Method for producing resin powder> Powdering methods for producing the resin powder of the present invention include melt granulation, in which a resin or resin composition (hereinafter sometimes referred to as "resin material") melted near its melting point is formed into fibers and then cut, and pulverization, in which the resin material is cut or destroyed by applying impact or shear. To improve the coatability of powder in powder bed fusion (PFB) molding, it is preferable that the resin powder of the present invention does not contain fine powder of around 10 μm and has a constant particle size and particle size distribution. Therefore, it is preferable to select a suitable powdering method so as to obtain powder of such a suitable shape.

[0054] As the pulverizing means, for example, a stamp mill, ring mill, stone mill, mortar, roller mill, jet mill, high-speed rotary mill, hammer mill, pin mill, container-driven mill, disk mill, media stirring mill, etc. can be used.

[0055] To prevent stretching of the resin material due to shear heating during milling, one method involves using liquid nitrogen or other cooling agents to cool the powder system, lowering the resin temperature during milling and producing powder through brittle fracture rather than ductile fracture. This method is called cryogenic milling or freeze milling. Among these, the use of a high-speed rotary mill for milling, which can produce powder with a particle size distribution and shape suitable for powder bed fusion (PFB) molding, is preferred because it improves fluidity and powder application during molding. Additionally, liquid nitrogen is preferred for producing powder from the resin material through brittle fracture, as this suppresses changes in the physical properties and color of the resin material due to milling.

[0056] From the viewpoint of increasing the circularity by removing elongated powder from the pulverized powder and from the viewpoint of removing fine powder and preventing the powder from flying up during handling, it is preferable to carry out a classification step after pulverization. In this case, classification methods include air classification, sieve classification, etc. If necessary, inorganic particles and reinforcing materials described below may be added and mixed with the obtained powder.

[0057] [Resin Powder (A)] The resin powder (A) of the present invention may be one type having the resin composition and physical properties shown below, or two or more types having different resin compositions or different physical properties may be mixed and used.

[0058] <Resin Composition of Resin Powder (A)> The resin (a) constituting the resin powder (A) used in the present invention is preferably a thermoplastic resin. The thermoplastic resin may be any material that exhibits thermoplasticity in response to the heat or light of the 3D printer device, and may be appropriately selected depending on the function to be imparted to the molded article to be formed.

[0059] As the thermoplastic resin for the resin powder (A), a commercially available thermoplastic resin material for three-dimensional modeling may be used. When a three-dimensional modeling material for a powder bed fusion method is used, the three-dimensional modeling material remaining after producing a model by the powder bed fusion method may be reused.

[0060] The three-dimensional modeling material of the present invention uses a combination of resin powder (A) and resin powder (B) described below, and can produce molded articles with excellent impact resistance while maintaining excellent modeling properties by using an existing resin powder for powder bed fusion as resin powder (A). However, the resin powder (A) used in the present invention is not limited to existing resin powders for powder bed fusion.

[0061] Examples of the resin (a) of the resin powder (A) include polyacetal, polyacrylate, polyacrylic acid, polyamide, polyamideimide, polyacid anhydride, polyarylate, polyarylene ether, polyarylene sulfide, polybenzoxazole, polyester, polyetheretherketone, polyetherimide, polyetherketoneketone, polyetherketone, polyethersulfone, polyimide, polymethacrylate, polyolefin, polyphthalide, polysilazane, polysiloxane, polystyrene, polysulfide, polysulfonamide, polysulfonate, polythioester, polytriazine, polyurea, polyurethane, polyvinyl alcohol, polyvinyl ester, polyvinyl ether, polyvinyl halide, polyvinyl ketone, polyvinylidene fluoride, polyvinyl aromatic, polysulfone, polyarylene sulfone, polyarylate, Examples of the thermoplastic elastomer include polyether ketone, polylactic acid, polyglycolic acid, poly-3-hydroxybutyrate, polyhydroxyalkanoate, starch, cellulose ester, poly(phenylene ether), poly(methyl methacrylate), styrene-acrylonitrile copolymer resin, poly(ethylene oxide), epichlorohydrin polymer, polycarbonate homopolymer, polycarbonate copolymer, poly(ester carbonate), poly(ester-siloxane-carbonate), poly(carbonate-siloxane), vinyl polymer, acrylonitrile-butadiene-styrene copolymer resin (ABS resin), methyl methacrylate-butadiene-styrene copolymer resin (MBS resin), polyvinyl chloride, olefin-based thermoplastic elastomer, styrene-based thermoplastic elastomer, polyurethane-based thermoplastic elastomer, and polyester-based thermoplastic elastomer.

[0062] Two or more of these resins may be mixed and used as appropriate.

[0063] Resin (a) may be appropriately mixed with fillers such as carbon black, carbon fiber, glass fiber, talc, mica, nanoclay, and magnesium, as well as additives such as antioxidants, lubricants, and colorants.

[0064] Of the thermoplastic resins listed above, polyolefin resins are preferred as resin (a), as they are particularly useful for a wide variety of articles, have good processability, and are recyclable.

[0065] <Polyolefin Resin> The polyolefin resin used in the present invention is a polymer obtained by polymerization of a monomer having a polyolefin skeleton. Polyolefin is a hydrocarbon resin having a carbon-carbon double bond.

[0066] The polyolefin resin is not particularly limited, and olefin homopolymers, block copolymers, random copolymers, etc. can be suitably used. Specific examples include polypropylene; propylene copolymers obtained by copolymerizing propylene with an α-olefin such as ethylene, 1-butene, 1-hexene, or 4-methyl-1-pentene; polyethylenes such as low-density polyethylene, linear low-density polyethylene, medium-density polyethylene, and high-density polyethylene; ethylene copolymers obtained by copolymerizing ethylene with an α-olefin such as 1-butene, 1-hexene, or 4-methyl-1-pentene; poly(1-butene), poly(4-methyl-1-pentene), etc. These may be used alone, or two or more types having different copolymer component compositions, physical properties, etc. may be mixed and used.

[0067] Among these, propylene polymers are particularly preferred as polyolefin resins from the viewpoint of obtaining molded articles with excellent heat resistance. Furthermore, from the viewpoint of moldability, propylene copolymers obtained by copolymerizing propylene with an α-olefin such as ethylene, 1-butene, 1-hexene, or 4-methyl-1-pentene are even more preferred, so as to suppress crystallization shrinkage during cooling and deformation such as warping of molded articles during molding. Here, the propylene copolymer is a polypropylene resin containing 50% by mass or more of propylene units among all monomer units.

[0068] Examples of the propylene copolymer include products manufactured by Japan Polypropylene Co., Ltd. under the trade names "Novatec (registered trademark) PP," "Wintec (registered trademark)," "Newcon (registered trademark)," and "Wellnex (registered trademark)," products manufactured by ExxonMobil Corporation under the trade name "Vistamax (registered trademark)," and products manufactured by The Dow Chemical Company under the trade name "Versify (registered trademark)." These products can be appropriately selected from the group of products and used alone or in combination of two or more.

[0069] As described above, the propylene copolymer may be a commercially available polypropylene resin material for three-dimensional modeling. When using a material for three-dimensional modeling for powder bed fusion (PFB), the material for three-dimensional modeling remaining after producing a molded body by PFB may be reused.

[0070] <Melting point and glass transition temperature of resin powder (A)> The resin powder (A) of the present invention preferably has a melting point or glass transition temperature of 50 ° C. or higher, more preferably 100 ° C. or higher. In addition, from the viewpoint of moldability for obtaining a molded body having excellent impact resistance using the resin powder (B) described later in a 3D printer, when the resin powder (B) is a thermoplastic resin, the resin powder (A) can be selected according to the thermal properties such as the melting point and crystallization temperature of the resin powder (B). However, the melting point (Tm) measured by differential scanning calorimetry (DSC) is preferably similar to that of the resin powder (A).

[0071] Specifically, the difference between the melting point (Tm) of resin powder (A) and the melting point (Tm) of resin powder (B) is preferably 70° C. or less, more preferably 40° C. or less, and even more preferably 20° C. or less. When the melting points (Tm) of resin powder (A) and resin powder (B) are similar in this way, both resins melt during powder bed fusion molding, allowing the resins to bond sufficiently to each other, and increasing the interlayer adhesion in the molded product, which is preferable.

[0072] <Average particle size (D50) of resin powder (A)> The average particle size (D50) of the resin powder (A) of the present invention depends on, for example, the specifications of the system used to form a resin molded body by a powder bed fusion method to which the material for three-dimensional modeling of the present invention is applied. However, from the viewpoint of applying the powder to a thickness within a predetermined range during modeling, the average particle size (D50) is usually 30 μm or more, preferably 35 μm or more, more preferably 40 μm or more, even more preferably 45 μm or more, and particularly preferably 50 μm or more, and is usually 250 μm or less, preferably 200 μm or less, more preferably 150 μm or less, and even more preferably 120 μm or less.

[0073] <Viscosity Average Molecular Weight (Mv) of Resin Powder (A)> The viscosity average molecular weight (Mv) of the resin powder (A) of the present invention is the viscosity average molecular weight (Mv) of the resin (a), and is preferably less than 500,000. A viscosity average molecular weight (Mv) of 500,000 or more is undesirable because the melt viscosity of the resin powder (A) increases, which may impair the spreadability and moldability of the molding material during powder bed fusion (PFB) molding. While the lower limit of the viscosity average molecular weight (Mv) of the resin powder (A) is not particularly limited, it is preferably 10,000 or more. If the viscosity average molecular weight of the resin powder (A) is less than 10,000, the mechanical strength of the molded body obtained by the PFB method may be insufficient, making it impossible to obtain a body with sufficient mechanical strength. From these perspectives, the viscosity average molecular weight (Mv) of the resin powder (A), i.e., the resin (a), is preferably 500,000 or less, and more preferably 450,000 or less. On the other hand, the viscosity average molecular weight (Mv) of the resin (a) is more preferably 50,000 or more, and even more preferably 100,000 or more.

[0074] [Resin Powder (B)] The resin powder (B) of the present invention is obtained using a thermoplastic resin or a thermosetting resin. The resin powder (B) may contain other resins, additives, reinforcing materials, etc., other than the thermoplastic resin or thermosetting resin, to the extent that the effects of the present invention are not impaired. Furthermore, commercially available three-dimensional modeling materials made of thermoplastic resins may be used as the resin powder (B). When using a three-dimensional modeling material for powder bed fusion (PFB) modeling, the three-dimensional modeling material remaining after producing a molded body by PFB may be reused.

[0075] The resin powder (B) may be used alone or in combination of two or more types having different physical properties such as resin composition, viscosity average molecular weight (Mv), and average particle size (D50).

[0076] <Resin Composition of Resin Powder (B)> The resin (b) constituting the resin powder (B) of the present invention can be appropriately selected depending on the function to be imparted to the molded article to be shaped.

[0077] In order to improve the impact resistance of the resulting molded body, the resin powder (B) according to the first and second embodiments of the present invention has an essential constituent requirement of being a resin composition different from that of the resin powder (A) of the present invention, and it is particularly preferable to use a resin having different thermal properties and mechanical properties.

[0078] In the third embodiment of the present invention, the resin powder (B) preferably has a resin composition different from that of the resin powder (A), and it is particularly preferable to use resins having different thermal characteristics and mechanical properties.

[0079] For example, resin (b) may be any resin that can be generally used as an impact modifier for resins. Specific examples include polyethylene, polypropylene, polyolefin copolymers, acrylate copolymers, acrylic acid copolymers, vinyl acetate copolymers, styrene copolymers, styrene block copolymers, ionic ethylene copolymers in which some of the acid groups are neutralized with metal ions, core-shell impact modifiers, and mixtures thereof. Among these, ultra-high molecular weight polyethylene, which has excellent impact resistance, is preferably used.

[0080] As the resin (b), not only the above-mentioned thermoplastic resins but also powders of thermosetting resins may be used. Examples of the thermosetting resin (b) include thermosetting elastomers. Specific examples include silicone rubber, fluororubber, acrylic rubber, urethane rubber, polyamide rubber, polysulfide rubber, and natural rubber.

[0081] Two or more of these resins may be mixed and used as appropriate.

[0082] Resin (b) may be appropriately mixed with fillers such as carbon black, carbon fiber, glass fiber, talc, mica, nanoclay, magnesium, and the like, and additives such as antioxidants, lubricants, and colorants.

[0083] <Ultra-high molecular weight polyethylene> The ultra-high molecular weight polyethylene suitably used as resin (b) of resin powder (B) of the present invention is preferably an ultra-high molecular weight polyethylene having a viscosity average molecular weight (Mv) of 500,000 or more and 10,000,000 or less. Ultra-high molecular weight polyethylene having a viscosity average molecular weight (Mv) of 500,000 or more is a polyethylene resin having an extremely large molecular weight and a linear molecular structure with almost no branched chains, and is known to have an excellent effect of imparting impact resistance.

[0084] If the viscosity average molecular weight (Mv) of the ultra-high molecular weight polyethylene is less than 500,000, the effect of the present invention, i.e., the effect of imparting impact resistance to molded articles obtained by a 3D printer, may not be achieved. From the viewpoint of imparting impact resistance, the viscosity average molecular weight (Mv) of the ultra-high molecular weight polyethylene used in the present invention is preferably 1 million or more, and more preferably 2 million or more. On the other hand, if the viscosity average molecular weight (Mv) of the ultra-high molecular weight polyethylene is excessively large, the fluidity of the ultra-high molecular weight polyethylene may be poor, which may impair the spreadability and modeling properties of the modeling material during powder bed fusion modeling. For this reason, the viscosity average molecular weight (Mv) of the ultra-high molecular weight polyethylene is 10 million or less, preferably 6 million or less, and more preferably 3 million or less.

[0085] Examples of commercially available ultra-high molecular weight polyethylene include those manufactured by Mitsui Chemicals under the trade names "Hizex Million (registered trademark)" and "Mipelon (registered trademark)," and those manufactured by Celanese Corporation under the trade name "GUR (registered trademark)."

[0086] <Melting Point (Tm) of Resin Powder (B)> Furthermore, the melting point (Tm) of resin powder (B) such as ultra-high molecular weight polyethylene, i.e., the melting point (Tm) of resin (b), is preferably 100 to 150° C., more preferably 120 to 140° C., for reasons of superior effects of the present invention. Furthermore, as described above, the melting point (Tm) of resin powder (B) is preferably close to the melting point (Tm) of resin powder (A).

[0087] <Particle size and particle size distribution of resin powder (A) and resin powder (B)> (Average particle size (D50) of resin powder (A) and resin powder (B) according to the first embodiment of the present invention) The average particle size (D50) of the resin powder (A) according to the first embodiment of the present invention depends on the specifications of the system used to form a resin molded body by a powder bed fusion method to which the material for three-dimensional modeling of the present invention is applied. However, from the viewpoint of applying the powder to a thickness within a predetermined range during modeling, the average particle size (D50) is usually 30 μm or more, preferably 35 μm or more, more preferably 40 μm or more, even more preferably 45 μm or more, and particularly preferably 50 μm or more, and is usually 250 μm or less, preferably 200 μm or less, more preferably 150 μm or less, and even more preferably 120 μm or less.

[0088] When used as a material for powder bed fusion, the resin powder (B) of the first embodiment of the present invention has an average particle size (D50) of less than 30 μm, so that the resin powder (B) is present between particles of the resin powder (A) and is easily contained in a model layer produced by melting and flowing the resin powder (A). That is, the average particle size (D50) of the resin powder (B) is smaller than that of the resin powder (A) having an average particle size (D50) of 30 μm or more and 250 μm.

[0089] If the average particle size (D50) of the resin powder (B) is less than 30 μm, this is preferable because it is smaller than the average particle size (D50) of the molding materials for the Powder Bed Fusion method, which usually have an average particle size (D50) of 30 μm or more and 250 μm or less.In this case, these molding materials can be suitably used as the resin powder (A), and there is a tendency for the uneven distribution of coarse particles to be reduced, resulting in good dispersion in the three-dimensional molding material of the present invention.This is preferable because the molding properties are maintained when molding a molded body using the Powder Bed Fusion method.

[0090] If the average particle size (D50) of the resin powder (B) is 30 μm or more, the resin powder (B) will not adhere to the surface of the resin powder (A) but will be present between the resin powders (A). In this case, in the molding process of a molded body by the powder bed fusion method, the resin powder (B) present between the resin powders (A) will inhibit the melting of the resin powder (A), making the molded body more likely to develop cracks and defects, which is undesirable. From this perspective, the average particle size (D50) of the resin powder (B) is preferably less than 30 μm, particularly 20 μm or less.

[0091] On the other hand, when the average particle size (D50) of the resin powder (B) is 1 μm or more, scattering and aggregation tend to be less likely to occur when the resin powder (B) is handled as a material for three-dimensional modeling or when the resin powder (B) is modeled. From this viewpoint, the average particle size (D50) of the resin powder (B) is preferably 5 μm or more, and more preferably 10 μm or more.

[0092] In particular, when ultra-high molecular weight polyethylene is used as the resin powder (B), if the average particle size (D50) of the resin powder (B) is smaller than 10 μm, the resin powder (B) will adhere to the surface of the resin powder (A), and the resin powder (B) will inhibit the melting of the resin powder (A), making it more likely that cracks and defects will occur in the three-dimensionally shaped product. Therefore, it is preferable that the average particle size (D50) of the ultra-high molecular weight polyethylene is 10 μm or more.

[0093] The average particle size (D50) of the resin powder (B) referred to in the present invention may be the average particle size of the particles before being made into a material for three-dimensional modeling, or the average particle size of particles dispersed in the material for three-dimensional modeling by melt-kneading or the like. As described above, the average particle size of the particles before being made into a material for three-dimensional modeling is the particle size (D50) at 50% of the frequency distribution of the powder in the particle size distribution detected by laser diffraction. Alternatively, the average particle size may be measured by an electrical resistance method. When the resin powder (B) is dispersed in the material for three-dimensional modeling, the average particle size may be obtained from 50 representative particles of the resin powder (B) enlarged with an optical microscope or the like. It has been confirmed that substantially equivalent values ​​are obtained with either average particle size.

[0094] In the first embodiment of the present invention, the ratio of the average particle size (D50) of the resin powder (B) to the average particle size (D50) of the resin powder (A) is preferably 3% or more and 30% or less. A ratio of 3% or more is preferred because it tends to suppress the generation of voids when mixing the resin powder (B) and the resin powder (A). A ratio of 5% or more is more preferred, and a ratio of 10% or more is even more preferred. Furthermore, a ratio of 30% or less tends to improve dispersion of the resin powder (B) among the resin powder (A), which is preferred because it maintains moldability during molding of a molded body by powder bed fusion. A ratio of 25% or less is more preferred, and a ratio of 20% or less is even more preferred. On the other hand, if the ratio exceeds 30%, the resin powder (B) does not adhere to the surface of the resin powder (A) and is present among the resin powder (A). In this case, in the molding process of a molded body by the Powder Bed Fusion method, the resin powder (B) present between the resin powders (A) may inhibit the melting of the resin powder (A), which may cause cracks or defects in the molded body.

[0095] (Average particle size (D50) of resin powder (A) and resin powder (B) according to the second embodiment of the present invention) For the same reasons as in the first embodiment of the present invention, the average particle size (D50) according to the second embodiment of the present invention is usually 30 μm or more, preferably 35 μm or more, more preferably 40 μm or more, even more preferably 45 μm or more, and particularly preferably 50 μm or more, and is usually 250 μm or less, preferably 200 μm or less, more preferably 150 μm or less, and even more preferably 120 μm or less.

[0096] For the same reasons as in the first embodiment of the present invention, in the second embodiment of the present invention, the ratio of the average particle size (D50) of the resin powder (B) to the average particle size (D50) of the resin powder (A) is 3% or more and 30% or less, preferably 5% or more and more preferably 10% or more, and on the other hand, preferably 25% or less and more preferably 20% or less.

[0097] Furthermore, for the same reasons as in the first embodiment of the present invention, in the second embodiment of the present invention, the average particle size (D50) of the resin powder (B) is preferably less than 30 μm, particularly preferably 20 μm or less, and is preferably 1 μm or more, more preferably 5 μm or more, and even more preferably 10 μm or more.

[0098] (Peak Tops of the Material for Three-Dimensional Modeling in a Third Embodiment of the Present Invention) In a third embodiment of the present invention, the material for three-dimensional modeling has, in a number-based particle size distribution chart obtained by image analysis, multiple peaks between 5 μm and 250 μm, a number-based peak in the region of 5 μm or more and less than 30 μm, and, in a volume-based particle size distribution chart obtained by image analysis, a volume-based peak top in the region of 5 μm or more and less than 30 μm, and the ratio of the number-based peak top to the volume-based peak top in the region of 5 μm or more and less than 30 μm (volume-based peak top / number-based peak top) is 2.5 or less, and the average particle size (D50) on a volume basis is 30 μm or more. The number-based peak top is preferably between 5 μm and 30 μm, and more preferably between 10 μm and 20 μm.

[0099] In the third embodiment of the present invention, the volumetric peak top is preferably between 5 μm and 30 μm, and more preferably between 10 μm and 20 μm. The ratio of the volumetric peak top to the numbertric peak top is 2.5 times or less, preferably 2.0 times or less, and more preferably 1.5 times or less. It is usually 1.0 times or more. When the ratio of the volumetric peak top to the numbertric peak top is equal to or less than the upper limit, the resin particles derived from the peak have a uniform particle size, resulting in excellent dispersibility in the material for three-dimensional modeling of the present invention.

[0100] When the peak tops on the number basis and the volume basis satisfy the above conditions, when the material is used as a material for Powder Bed Fusion (PFB), other particles exist between the particles, and the small-diameter particles tend to be contained in the layer of the object produced by melting and flowing. Furthermore, uneven distribution of coarse particles tends to be reduced, leading to good dispersion in the material for three-dimensional modeling of the present invention. This is preferable because the formability is maintained when a molded object is formed by Powder Bed Fusion (PFB).

[0101] In the third embodiment of the present invention, the average particle size (D50) on a volume basis is 30 μm or more, preferably 35 μm or more, more preferably 40 μm or more, and is usually 120 μm or less.

[0102] <Content of Resin Powder (A) and Resin Powder (B)> The content of resin powder (B) in the three-dimensional modeling material of the present invention may be selected to provide sufficient impact resistance and moldability required for the resulting molded body. Specifically, from the viewpoint of imparting impact resistance, the content of resin powder (B) is preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more relative to the total amount of resin powder (A) and resin powder (B). Furthermore, from the viewpoint of moldability, the content of resin powder (B) is preferably less than 50% by mass, more preferably 45% by mass or less, and even more preferably 40% by mass or less. Setting the content of resin powder (B) to the above upper limit or less prevents the occurrence of areas in which the molten resin does not flow within each layer during the three-dimensional modeling process, does not reduce interlayer adhesion, and is preferable from the viewpoint of maintaining moldability and the mechanical properties of the resulting molded body.

[0103] [Other Components] In addition to the resin powders (A) and (B) of the present invention, the three-dimensional modeling material of the present invention may contain, as appropriate, commonly used additives within a range that does not significantly impair the effects of the present invention. Examples of the additives include inorganic particles such as silica, alumina, and kaolin, organic particles such as acrylic resin particles and melamine resin particles, pigments such as titanium oxide and carbon black, weather resistance stabilizers, heat resistance stabilizers, antistatic agents, electromagnetic wave absorbers, melt viscosity modifiers, crosslinkers, lubricants, nucleating agents, plasticizers, antioxidants, antioxidants, light stabilizers, UV absorbers, neutralizers, antifogging agents, antiblocking agents, slip agents, and colorants, which are added for the purpose of improving or adjusting the modeling properties, the stability of the three-dimensional model, and the physical properties of the three-dimensional model.

[0104] The content of these additives is not particularly specified, but from the viewpoint of the stability of the resulting three-dimensional modeling material and the three-dimensional model formed therefrom, the total amount of additives is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, even more preferably 0.08 parts by mass or more, and particularly preferably 0.1 parts by mass or more, per 100 parts by mass of the total three-dimensional modeling material. Furthermore, from the viewpoint of suppressing a decrease in interlayer adhesion of the molded body to be modeled, the upper limit of the total content of additives is preferably 30 parts by mass or less, more preferably 28 parts by mass or less, and even more preferably 25 parts by mass or less.

[0105] In addition to the additives described above, the three-dimensional modeling material of the present invention may contain a reinforcing material that is generally blended as appropriate, within a range that does not significantly impair the effects of the present invention.

[0106] Specific examples of reinforcing materials include inorganic fillers and inorganic fibers. Specific examples of inorganic fillers include calcium carbonate, zinc carbonate, magnesium oxide, calcium silicate, sodium aluminate, calcium aluminate, sodium aluminosilicate, magnesium silicate, potassium titanate, glass balloons, glass flakes, glass powder, silicon carbide, silicon nitride, boron nitride, gypsum, calcined kaolin, zinc oxide, antimony trioxide, zeolite, hydrotalcite, wollastonite, silica, talc, mica, nanocloy, metal powders such as magnesium, alumina, graphite, carbon black, and carbon nanotubes. Specific examples of inorganic fibers include cut glass fiber, milled glass fiber, glass fiber, gypsum whiskers, metal fiber, metal whiskers, ceramic whiskers, carbon fiber, and cellulose nanofibers.

[0107] The content of these reinforcing materials in the three-dimensional modeling material of the present invention is not particularly limited, but from the viewpoint of the strength of the molded body to be modeled, it is preferably 1 part by mass or more, more preferably 5 parts by mass or more, and even more preferably 10 parts by mass or more, per 100 parts by mass of the three-dimensional modeling material in total. Furthermore, from the viewpoint of suppressing a decrease in interlayer adhesion of the molded body to be modeled, the content of these reinforcing materials in the three-dimensional modeling material is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, and even more preferably 30 parts by mass or less.

[0108] [Method for Producing a Material for Three-Dimensional Modeling] The material for three-dimensional modeling of the present invention can be produced by adding and mixing the resin powder (A) and resin powder (B) of the present invention with the other additives and reinforcing materials, etc., which are blended as needed, in a predetermined ratio. The method for producing the material for three-dimensional modeling of the present invention is not particularly limited as long as it contains each component. For example, the material for three-dimensional modeling of the present invention can be produced by pre-mixing the resin powder (A) and resin powder (B) of the present invention with other components, such as additives and reinforcing materials, which are blended as needed, using various mixers such as a tumbler or a Henschel mixer, and then melt-kneading the mixture using a Banbury mixer, roll, Brabender, single-screw kneading extruder, twin-screw kneading extruder, kneader, etc.

[0109] [Average particle size (D50) of the material for three-dimensional modeling] The material for three-dimensional modeling of the present invention is preferably in powder form containing the resin powder (A) and resin powder (B) of the present invention, and other additives, reinforcing materials, etc., which are blended as necessary, as a material for three-dimensional modeling by the powder bed fusion method. In this case, the average particle size (D50) of the powder for three-dimensional modeling of the present invention is preferably larger than the average particle size (D50) of the resin powder (B). From this viewpoint, the average particle size (D50) of the powder for three-dimensional modeling of the present invention is preferably 3 to 30 times, particularly 5 to 20 times, the average particle size (D50) of the resin powder (B).

[0110] Specifically, when the powder for three-dimensional modeling of the present invention is used as a material for the Powder Bed Fusion method, the average particle size (D50) depends on the specifications of the system used to form the molded body by the Powder Bed Fusion method, but from the viewpoint of applying the powder to a thickness within a predetermined range during modeling, it is preferably 20 μm or more, more preferably 30 μm or more, even more preferably 40 μm or more, particularly preferably 50 μm or more, and most preferably 55 μm or more, and is preferably 250 μm or less, more preferably 200 μm or less, even more preferably 150 μm or less, and particularly preferably 120 μm or less.

[0111] [Molded Article] The molded article of the present invention is made from the above-described material for three-dimensional modeling of the present invention. As a method for producing the molded article of the present invention, molding is preferably performed using a three-dimensional printer. The detailed production method is described below.

[0112] [Method for manufacturing a molded body] In the method for manufacturing a molded body made from the material for three-dimensional modeling of the present invention, the material for three-dimensional modeling of the present invention is used and molded using a three-dimensional printer to obtain a molded body. Examples of molding methods using a three-dimensional printer include powder bed fusion and multi-jet fusion. Among these, in the present invention, powder bed fusion, in which the modeling material is in powder form, is preferably used.

[0113] In the Powder Bed Fusion method, particles of a material for 3D modeling spread on a stage are irradiated with a laser or electron beam to sinter or fuse the particles and form a layer in the vertical direction. Next, particles of the material for 3D modeling are spread in contact with the layer formed above and irradiated with a laser or electron beam to form the next layer. By successively stacking layers in this way, a molded body of the desired shape can be obtained.

[0114] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the present invention.

[0115] [Methods for measuring and evaluating physical properties] <Average particle size (D50)> Five grams of powder material was weighed, and the particle size distribution of the powder was measured on a volume basis using a particle size distribution analyzer (manufactured by Horiba, Ltd.) that uses laser diffraction. The particle size at 50% of the frequency distribution of the powder in the detected particle size distribution was determined as the average particle size (D50). However, for commercially available products, some catalog values ​​were used. (This value is considered to be equivalent to the value measured using the above measurement method.)

[0116] <Particle size distribution charts based on number and volume by image analysis> 1 cc of powder sample was spread on a glass slide and observed using a particle size distribution analyzer equipped with particle size analysis software on a microscope with an analysis function, and particle size analysis was performed under the following particle size analysis conditions. The particle size distribution was determined based on the number or volume of the equivalent circle diameter calculated from the area of ​​the obtained particle image, and a chart was created. (Observation conditions) Measuring device: XploRA Plus manufactured by HORIBA, Ltd. Observation illumination: transmitted light Objective lens: Olympus bright / dark field plan achromat MPLN 10 xBD Observation field: 15 x 11 mm area (composite image of 17 x 15 fields of view) (Particle size analysis conditions) Particle size analysis software: Particle Finder ver. 2 Particle size cutoff: equivalent circle diameter of 4 μm or more Circularity cutoff: circularity of 0.6 or more Distribution criteria: number distribution and volume distribution

[0117] <Volume-Based Average Particle Size (D50) by Image Analysis> The particle size at 50% of the powder frequency distribution in the volume-based particle size distribution obtained by image analysis as described above was determined as the average particle size (D50).

[0118] <Viscosity Average Molecular Weight (Mv)> For the ultra-high molecular weight polyethylene used as the resin powder (B), the viscosity average molecular weight (Mv) was calculated according to the method specified in ASTM D4020 using the specific viscosity ηsp (dl / g) of a 0.05% decalin solution at 135°C instead of the intrinsic viscosity [η] (dl / g) according to the following formula (I): Mv = 5.37 × 10 4 ηsp 1.37 ...(I)

[0119] <Melting Point (Tm)> The melting points (Tm) of resin powder (A) and resin powder (B) were measured by the following method. Using a differential scanning calorimeter (Pyris1 DSC) manufactured by PerkinElmer Co., Ltd., in accordance with JIS K7121, approximately 10 mg of a powder sample was heated from room temperature to 200°C at a heating rate of 10°C / min, held at that temperature for 1 minute, cooled to 50°C at a heating rate of 10°C / min, and then heated again to 200°C at a heating rate of 10°C / min. The crystalline melting temperature (melting point: Tm) (°C) (reheating process) showing the maximum peak in the melting curve detected from the measured thermogram was determined. The measured values ​​were rounded to one decimal place.

[0120] <Dispersibility> 0.3 g of a powder sample for 3D modeling was placed in a recess of a table measuring 25 mm x 30 mm and 0.2 mm deep, and a roller was then rolled on the table at a speed of approximately 64 mm / sec to level the powder in the recess. Dispersibility was evaluated based on the state of the powder filled in the recess according to the following criteria: A: The powder was uniformly dispersed. B: The powder was not uniformly dispersed, or there was clumping of powder particles.

[0121] <Formability> Using a powder bed fusion printer Lisa Pro (Sinterit), the printing area (Print bed) was set to a temperature above the crystallization temperature and below the crystal melting temperature of the powder sample for 3D printing, and the material supply section (Feed bed) was set to a temperature above the crystallization temperature of the powder sample. Under the condition of a layer pitch of 0.125 mm, a test piece having a length of 80 mm, a width of 12.7 mm, a thickness of 5 mm, and a V-notch of 2 mm was produced by forming the thickness direction of the test piece as the layering direction, and the appearance of the test piece was observed to determine whether or not there were any molding defects. The formability was evaluated according to the following criteria. A: Formable, and mechanical properties could be evaluated using the obtained test piece. B: Formable, but very brittle. Or, molding defects such as chipping were observed.

[0122] <Impact Resistance> The Charpy impact strength of the test pieces prepared for the evaluation of moldability was measured in accordance with JIS K7111-1. A Charpy impact test was performed on these test pieces at a measurement temperature of 25°C, a hammer capacity of 4J, and with the striking surface opposite the notch, to measure the Charpy impact value. The impact resistance of each test piece was calculated as a ratio to the Charpy impact value of Comparative Example 1, in which only propylene copolymer powder was used as the molding material, and evaluated from this ratio according to the following criteria: AA: Charpy impact value ratio of 120% or more; A: Charpy impact value ratio of more than 100% but less than 120%; B: Charpy impact value ratio of 100% or less.

[0123] <Overall Evaluation> The above evaluation results were evaluated according to the following criteria: AA: All were "A" or higher, and at least one was "AA" A: All were "A" B: At least one was "B"

[0124] [Example 1] Resin powder (A), propylene copolymer powder (manufactured by Sinterit) (A-1) (Tm: 135 ° C., D50: 87 μm) 90 parts by mass of powder material for LisaPro 3D printers, resin powder (B), ultra-high molecular weight polyethylene Mipelon (registered trademark) PM-200 (manufactured by Mitsui Chemicals, Inc.) (B-1) (Mv: 1.8 million, Tm: 137 ° C., D50: 10 μm) 10 parts by mass was added and dry blended, carbon powder as an electromagnetic wave absorber (fine powder SGP-10, manufactured by SEC Carbon Co., Ltd., average particle size 10 μm) was mixed with 0.3 parts by mass of resin powder (B) 100 parts by mass to obtain a powder for three-dimensional modeling (D50: 79 μm). The results of the above-mentioned evaluation using the obtained powder for three-dimensional modeling are shown in Table 1. FIG. 1 shows a particle size distribution chart based on the number of particles obtained by image analysis of this powder for three-dimensional modeling, and FIG. 2 shows a particle size distribution chart based on the volume of particles obtained by image analysis of this powder for three-dimensional modeling.

[0125] Example 2 A powder for three-dimensional modeling (D50: 79 μm) was obtained in the same manner as in Example 1, except that silicone powder KMP-597 (manufactured by Shin-Etsu Chemical Co., Ltd.) (B-2) (D50: 5 μm) was used instead of Mipelon (registered trademark) PM-200 (manufactured by Mitsui Chemicals, Inc.) (B-1). The results of the above-mentioned evaluation using the obtained powder for three-dimensional modeling are shown in Table 1. Furthermore, a graph of a particle size distribution chart on a number basis, obtained by image analysis of this powder for three-dimensional modeling, is shown in FIG. 3, and a graph of a particle size distribution chart on a volume basis is shown in FIG. 4.

[0126] Example 3 A powder for 3D modeling (D50: 70 μm) was obtained in the same manner as in Example 1, except that 20 parts by mass of Mipelon (registered trademark) PM-200 (manufactured by Mitsui Chemicals, Inc.) (B-1) was added to 80 parts by mass of a propylene-based copolymer powder (manufactured by Sinterit) (A-1). The results of the above-mentioned evaluations performed using the obtained powder for 3D modeling are shown in Table 1. Furthermore, a graph of a particle size distribution chart on a number basis, obtained by image analysis of this powder for 3D modeling, is shown in FIG. 5, and a graph of a particle size distribution chart on a volume basis is shown in FIG. 6.

[0127] [Example 4] As the resin powder (A), a polyamide powder (manufactured by Sinterit) (A-2) (Tm: 185 ° C., D50: 38 μm) of powder material for LisaPro 3D printers was used, and as the resin powder (B), KynarFlex (registered trademark) 3121-50 (manufactured by Arkema) (B-3) (Tm: 165 ° C., D50: 10 μm) was used. Except for this, a powder for 3D modeling (D50: 34 μm) was obtained in the same manner as in Example 1. The results of the above-mentioned evaluation using the obtained powder for 3D modeling are shown in Table 1. In addition, a graph of the particle size distribution chart on a number basis obtained by image analysis of this powder for 3D modeling is shown in FIG. 7, and a graph of the particle size distribution chart on a volume basis is shown in FIG. 8.

[0128] [Comparative Example 1] Ultra-high molecular weight polyethylene was not used, and only propylene copolymer powder (manufactured by Sinterit) (A-1) was used as a powder material for LisaPro 3D printers. Since the propylene copolymer powder (manufactured by Sinterit) (A-1) used as a powder material for LisaPro 3D printers contains a laser absorber, adding and mixing carbon powder was not necessary. The results of the above-mentioned evaluation using the obtained powder for 3D modeling are shown in Table 1. Furthermore, a graph of the particle size distribution chart on a number basis obtained by image analysis of this powder for 3D modeling is shown in Figure 9, and a graph of the particle size distribution chart on a volume basis is shown in Figure 10.

[0129] Comparative Example 2 A powder for 3D modeling (D50: 81 μm) was obtained in the same manner as in Example 1, except that Mipelon (registered trademark) XM-220U (C-1) (Mv: 2 million, Tm: 136°C, D50: 30 μm) was used instead of Mipelon (registered trademark) PM-200 (manufactured by Mitsui Chemicals, Inc.) (B-1). The results of the above-mentioned evaluation using the obtained powder for 3D modeling are shown in Table 1. FIG. 11 is a graph of a particle size distribution chart on a number basis, and FIG. 12 is a graph of a particle size distribution chart on a volume basis, obtained by image analysis of this powder for 3D modeling.

[0130] Comparative Example 3 A powder for 3D modeling (D50: 80 μm) was produced in the same manner as in Example 1, except that a propylene copolymer powder (produced by Japan Polypropylene Corporation, powdered Wintec WFX4M, Tm: 127°C) (C-2) (D50: 18 μm) was used instead of Mipelon (registered trademark) PM-200 (produced by Mitsui Chemicals, Inc.) (B-1). The results of the above-mentioned evaluation using the obtained powder for 3D modeling are shown in Table 1. FIG. 13 is a graph showing a particle size distribution chart on a number basis, and FIG. 14 is a graph showing a particle size distribution chart on a volume basis, obtained by image analysis of this powder for 3D modeling.

[0131]

[0132] As is clear from the above results, a three-dimensional modeling material containing two types of resin powder (A) and resin powder (B) with different resin compositions and particle sizes, in which the particle sizes or particle size distributions of resin powder (A) and resin powder (B) satisfy the specifications of the present invention, is found to have excellent modeling properties in a 3D printer and excellent impact resistance of the resulting molded body.

[0133] Although the present invention has been described in detail using specific embodiments, it will be apparent to those skilled in the art that various modifications are possible within the scope of the effects of the invention. In particular, the first, second, and third preferred embodiments can be arbitrarily combined. This application is based on Japanese Patent Application No. 2023-058527, filed on March 31, 2023, and is incorporated by reference in its entirety.

[0134] The three-dimensional modeling material of the present invention can provide a three-dimensional modeling material that has excellent impact resistance for molded articles produced by a 3D printer, while maintaining the modeling ability and safety of the powder material, even when using existing resin powders for powder bed fusion. Therefore, the three-dimensional modeling material of the present invention can be used not only for prototypes, but also for practical applications such as components for home appliances, building materials, aircraft, and automotive materials.

Claims

1. A material for three-dimensional modeling comprising: a resin powder (A) having an average particle size (D50) measured by a laser diffraction method of 30 μm or more and 250 μm or less; and a resin powder (B) having a resin composition different from that of the resin powder (A) and having an average particle size (D50) measured by a laser diffraction method of 1 μm or more and less than 30 μm.

2. The material for three-dimensional modeling according to claim 1, wherein the average particle size (D50) of the resin powder (B) is 3% or more and 30% or less of the average particle size (D50) of the resin powder (A).

3. A material for three-dimensional modeling comprising: a resin powder (A) having an average particle size (D50) of 30 μm or more and 250 μm or less as measured by a laser diffraction method; and a resin powder (B) having a resin composition different from that of the resin powder (A) and having an average particle size (D50) of 3% or more and 30% or less of the average particle size (D50) of the resin powder (A) as measured by a laser diffraction method.

4. A material for three-dimensional modeling, characterized in that in a particle size distribution chart on a number basis obtained by image analysis using the following method, it has multiple peaks between 5 μm and 250 μm, and has at least one peak top in the region of 5 μm or more and smaller than 30 μm, and in a particle size distribution chart on a volume basis obtained by image analysis, it has a peak top in the region of 5 μm or more and smaller than 30 μm, the value of the volumetric peak top is 2.5 times or less than the value of at least one number-based peak top, and the average particle size (D50) on a volume basis is 30 μm or more. Image analysis method: 1 cc of resin powder is spread on a slide, and observation is performed under the following observation conditions, and particle size analysis is performed under the following particle size analysis conditions. (Observation conditions) Measuring device: XploRA Plus manufactured by HORIBA, Ltd. Observation illumination: transmitted light Objective lens: Olympus bright / dark field plan achromat MPLN 10 xBD Observation field: 15 x 11 mm area (composite image of 17 x 15 fields of view) (Particle size analysis conditions) Particle size analysis software: Particle Finder ver. 2 Particle size cutoff: equivalent circle diameter 4 μm or more Circularity cutoff: circularity 0.6 or more Distribution criteria: number distribution and volume distribution 5. The material for three-dimensional modeling according to claim 4, comprising a resin powder (A) and a resin powder (B), the resin composition of the resin powder (B) being different from the resin composition of the resin powder (A).

6. The material for three-dimensional modeling according to any one of claims 1 to 3 and 5, wherein the resin powder (A) is a powder of a polyolefin-based resin.

7. The material for three-dimensional modeling according to claim 6, wherein the polyolefin resin is a propylene polymer.

8. The material for three-dimensional modeling according to any one of claims 1 to 3 and 5 to 7, wherein the resin powder (B) is a powder of at least one of polyethylene and a thermosetting elastomer.

9. The material for three-dimensional modeling according to claim 8, wherein the viscosity average molecular weight (Mv) of the polyethylene is 500,000 or more and 10,000,000 or less.

10. A material for three-dimensional modeling according to any one of claims 1 to 3 and 5 to 9, wherein the content of the resin powder (B) is 1 mass % or more and less than 50 mass % with respect to the total amount of the resin powder (A) and the resin powder (B).

11. The material for three-dimensional modeling according to any one of claims 1 to 10, which is in powder form.

12. The material for three-dimensional modeling according to any one of claims 1 to 11, which is a material for three-dimensional modeling by a Powder Bed Fusion method.

13. A molded product obtained by using the material for three-dimensional modeling according to any one of claims 1 to 12.

14. A method for producing a molded body, comprising a step of three-dimensionally molding a molded body by a Powder Bed Fusion method using the material for three-dimensional molding according to any one of claims 1 to 12.

Citation Information

Patent Citations

  • Resin powder, resin powder for solid molding, method for manufacturing solid molded article, and apparatus for manufacturing solid molded article

    JP2021146678A

  • Powder materials for 3D printers, three-dimensional objects and their manufacturing methods

    JP7369326B2

  • Polyarylene sulfide resin powder granular article mixture and method for producing three-dimensional molded article

    WO2018074353A1

Cited By

  • Resin particle composition for 3D printer and method for producing resin particle composition for 3D printer

    WO2026105807A1