Carbon electrode material and redox flow battery provided with same
The carbon electrode material with unevenly distributed carbonized binder and carbon particles addresses the challenges of electrode resistance and short circuits in redox flow batteries, enhancing energy efficiency and cost-effectiveness by reducing cell resistance and preventing self-discharge.
Patent Information
- Application Number
- PCT/JP2024/012282
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
Redox flow batteries face challenges in reducing electrode resistance and preventing short circuits while maintaining high liquid permeability, which affects energy efficiency and cost-effectiveness.
A carbon electrode material with a carbonized binder and carbon particles unevenly distributed on both surfaces of the carbon fiber layer, providing a surface aperture ratio of 30-50% and a thickness of 1-5 mm, which reduces cell resistance and prevents short circuits.
The solution achieves low resistance and high liquid permeability, reducing energy loss and self-discharge, making it suitable for vanadium-based redox flow batteries and other energy storage systems.
Smart Images

Figure JP2024012282_03102024_PF_FP_ABST
Abstract
Description
Carbon electrode material and redox flow battery including the same
[0001] The present invention relates to a carbon electrode material used in a redox battery, and more particularly to a carbon electrode material that is excellent in the overall energy efficiency of a redox flow battery.
[0002] Redox flow batteries utilize the oxidation-reduction reaction of redox ions in an aqueous solution while circulating (flowing) an electrolyte within the cell. Because the reaction is mild and occurs only in the liquid phase, they are extremely safe, large-capacity storage batteries.
[0003] The electrolyte used in redox flow batteries can be an aqueous solution of iron, chromium, or the like, whose valence can be changed by oxidation-reduction. Typically, an acidic aqueous solution of vanadium oxysulfate is widely used as the positive electrode electrolyte, and an acidic aqueous solution of vanadium sulfate is widely used as the negative electrode electrolyte.
[0004] Redox flow batteries are highly safe and offer excellent benefits for scaling up, but reducing the cost of batteries is highly desirable for widespread use. Generally, the cost of batteries can be reduced by selecting inexpensive, general-purpose materials. On the other hand, the development of high-performance cell components (electrodes, ion exchange membranes, current collector plates, etc.) can reduce the amount of materials used and running costs, contributing to cost reductions.
[0005] Among these, electrode materials for redox flow batteries are extremely important cell components, as they not only function as reaction sites for ions but also as flow paths for the electrolyte. If electrode materials can be given low resistance and high liquid permeability, battery efficiency and system efficiency can be improved, which will ultimately contribute significantly to cost reductions for redox flow batteries (see Patent Documents 1 to 6).
[0006] JP 2017-33758 A JP 2018-147595 A International Publication WO2019 / 049755 International Publication WO2015 / 032667 JP 2014-207240 A JP 2016-178094 A
[0007] To further reduce the resistance of electrodes, it is effective to minimize the interelectrode distance and the electron conduction path, and the trend is to use thinner electrodes. However, thinner electrodes increase the pumping power loss when passing the electrolyte, reducing system efficiency. In this case, methods to reduce pumping power loss by forming flow channels on the current collector plate side have also been investigated. However, this not only increases the processing costs on the current collector plate side, but also increases the number of flow channels that are not involved in oxidation-reduction. Forming flow channels on the current collector plate side is not always appropriate. Therefore, it can be said that there is great technological significance in imparting high liquid permeability while expressing low resistance in carbon electrode materials.
[0008] Another approach to reducing resistance is to reduce the thickness of the ion-exchange membrane. However, reducing the thickness of the membrane significantly increases the possibility that the fibers of the carbon electrode material and the irregularities of the carbonized binder will penetrate the membrane, causing a short circuit between the two electrodes. If a short circuit occurs, self-discharge will significantly reduce battery efficiency, eliminating the benefit of reducing the thickness. Therefore, when reducing the thickness of the ion-exchange membrane, it is also necessary to impart properties to the carbon electrode material that make the membrane less susceptible to destruction.
[0009] To address the above-mentioned technical issues, for example, Patent Document 1 discloses that low-crystallinity carbon particles can be supported by a phenolic resin to reduce resistance. However, this only applies a commercially available dispersion liquid (manufactured by Lion Corporation), and although it has the effect of reducing resistance, it is difficult to say that the design takes into consideration high liquid permeability and short-circuit prevention.
[0010] In addition, Patent Document 2 discloses that the optimum specific surface area when using a carbon paper fiber substrate and graphite is 0.5 to 1.5 m 2 However, although Patent Document 2 is characterized by the fact that it can be made thinner than conventional carbon fiber nonwoven fabrics and is inexpensive, it is not designed to achieve both low resistance and high liquid permeability.
[0011] Patent Documents 3 and 4 disclose that high-specific-surface-area carbon particles can be supported by a highly crystalline carbonized binder, thereby further reducing resistance. However, these designs also do not seem to take into consideration high liquid permeability or the prevention of short circuits.
[0012] Patent Document 5 proposes a method of forming an area where resin carbide is unevenly distributed near the surface layer of carbon fiber paper to reduce contact resistance with adjacent members. However, Patent Document 5 exemplifies that it is preferable that fibers and voids other than those on the outermost surface are almost invisible when the surface is observed, and the surface opening ratio mentioned in the present invention is extremely low, so it is thought that this does not achieve both low resistance and short circuit suppression as a carbon electrode material for redox batteries.
[0013] Furthermore, Patent Document 6 proposes a carbon sheet with gas diffusivity and drainage properties, in which the difference in surface coverage between one side X2 and the other side Y2 of the carbon fiber and binder is 5% or more and 20% or less. However, the surface coverages of both X2 and Y2 in each example exceed approximately 70%, which is considered to be insufficient to satisfy the surface opening ratio mentioned in the present invention. Furthermore, considering that the sheet is not subjected to an activation treatment effective in redox batteries and is treated with a water repellent, it is unsuitable as a carbon electrode material for redox batteries. Furthermore, because the fiber structure is paper, it can only be applied to ultra-thin redox flow batteries with flow channels formed in the current collector plate.
[0014] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a carbon electrode material for a redox flow battery that can not only reduce cell resistance during initial charge and discharge to increase battery energy efficiency, but also reduce energy loss during solution transfer and increase system efficiency.
[0015] The carbon electrode material for a redox flow battery according to the present invention, which has been able to solve the above problems, has the following configuration.
[0016] The present invention is configured as follows. (1) A carbon electrode material for a redox flow battery, characterized in that a carbonized binder and carbon particles are unevenly distributed on both surfaces of a carbon fiber layer, the number of oxygen atoms bonded to carbon atoms on the surface is 1.0 atomic % or more of the total number of carbon atoms on the surface, a surface opening ratio determined by binarizing a microscopic image acquired with an electron microscope is 30 to 50%, and the thickness is 1 to 5 mm. (2) The carbon electrode material described in (1) above, characterized in that a part or all of the carbonized binder is present inside the carbon fiber layer. (3) The carbon electrode material described in (1) or (2) above, in which the average fiber diameter of the fibers constituting the carbon fiber layer is 10 to 30 μm. (4) A redox flow battery using the carbon electrode material described in any one of (1) to (3) above as an electrode.
[0017] According to the present invention, not only is cell resistance during initial charge and discharge reduced, resulting in excellent battery energy efficiency, but high liquid permeability also reduces energy loss in the liquid pump, resulting in excellent system efficiency. Furthermore, due to its resistance to short circuits, a carbon electrode material suitable for use in vanadium-based redox flow batteries with low energy loss due to self-discharge is obtained. The carbon electrode material of the present invention is suitable for use in flow-type and non-flow-type redox flow batteries, or redox flow batteries combined with lithium, capacitor, and fuel cell systems.
[0018] 1 is a schematic diagram of a redox flow battery used in the present invention; FIG. 2 is a diagram showing a single cell of a redox flow battery using an electrode material of the present invention; FIG. 3 is a microscopic image of the surface of Example No. 1 obtained by an electron microscope; FIG. 4 is a microscopic image of the surface of Comparative Example No. 7 obtained by an electron microscope; FIG. 5 is a microscopic image of the surface of Comparative Example No. 8 obtained by an electron microscope; FIG. 6 is a microscopic image of the cross section of Example No. 1 obtained by an electron microscope; and FIG. 7 is a microscopic image of the cross section of Comparative Example No. 7 obtained by an electron microscope.
[0019] The present inventors have conducted extensive research to provide a carbon electrode material that is particularly suitable for use in vanadium-based redox flow batteries. In vanadium-based redox flow batteries, it is important to achieve both low resistance and high electrolyte permeability from the standpoint of cost reduction, as well as to suppress short circuits.
[0020] Hereinafter, the present invention will be described in detail for each of its constituent elements with reference to FIGS.
[0021] FIG. 1 is a schematic diagram of a redox flow battery using a carbon electrode material 5 (hereinafter simply referred to as electrode material 5) of the present invention. FIG. 2 is a diagram showing an example of a unit cell of a redox flow battery using the electrode material 5 of the present invention. In the unit cell, an ion exchange membrane 3 is disposed between two opposing current collector plates 1, 1, and electrolyte passages 4a, 4b are formed on both sides of the ion exchange membrane 3 by spacers 2 along the inner surfaces of the current collector plates 1, 1. An electrode material 5 is disposed in at least one of the passages 4a, 4b. The current collector plate 1 is provided with a liquid inlet 10 and a liquid outlet 11 for the electrolyte. As shown in FIG. 1 , the electrode is composed of the electrode material 5 and the current collector plate 1, and the electrolyte passes through the electrode material 5 (a three-dimensional electrode structure).
[0022] In the electrode material 5 of the present invention, the carbonized binder and carbon particles are unevenly distributed on both surfaces of the carbon fiber layer, the surface opening ratio determined by binarization of a microscopic image acquired by an electron microscope is 30 to 50%, and the thickness of the electrode material 5 is 1 to 5 mm. The electrode material 5 is an electrode material 5 that combines low resistance and high liquid permeability and suppresses short circuits. Here, "the carbonized binder is unevenly distributed on both surfaces" means that there is more carbonized binder on both surfaces than in the carbon fiber layer (the center in the thickness direction of the carbon fiber layer), and "the carbon particles are unevenly distributed on both surfaces" means that there are more carbon particles on both surfaces than in the carbon fiber layer (the center in the thickness direction of the carbon fiber layer). The uneven distribution can be confirmed by a microscopic image of the cross section of the electrode material 5 acquired by an electron microscope, as will be described in detail below.
[0023] [Carbon Fiber] In the electrode material 5 of the present invention, the carbon fiber constituting the carbon fiber layer is a fiber obtained by subjecting an organic fiber precursor to a thermal carbonization treatment (details will be described later), and refers to a fiber composed of 90% or more by mass of carbon (JIS L 0204-2). Examples of organic fiber precursors that can be used as raw materials for carbon fibers include acrylic fibers such as polyacrylonitrile; phenolic fibers; PBO fibers such as polyparaphenylene benzobisoxazole (PBO); aromatic polyamide fibers; pitch fibers such as isotropic pitch fibers, anisotropic pitch fibers, and mesophase pitch; and cellulose fibers. Among these, from the viewpoint of excellent strength and elastic modulus, acrylic fibers, phenolic fibers, cellulose fibers, isotropic pitch fibers, and anisotropic pitch fibers are preferred as organic fiber precursors, with acrylic fibers being more preferred. The acrylic fiber is not particularly limited as long as it contains acrylonitrile as the main component. However, the acrylonitrile content of the raw material monomers forming the acrylic fiber is preferably 95% by mass or more, and more preferably 98% by mass or more.
[0024] The average fiber diameter of the carbon fibers is preferably 10 to 30 μm. If the average fiber diameter is smaller than 10 μm, the liquid permeability will be reduced. On the other hand, if the average fiber diameter is larger than 30 μm, the surface area will be reduced, and even if carbon particles are supported, the cell resistance will be high. Considering the balance between liquid permeability and reaction surface area, the diameter is more preferably 10 to 25 μm.
[0025] In the electrode material 5 of the present invention, it is preferable to use the above-mentioned carbon fiber as a substrate for the carbon fiber layer, which improves the strength of the carbon fiber layer and makes it easier to handle and process. Specific examples of the substrate include spun yarn, filament bundle yarn, nonwoven fabric, knitted fabric, woven fabric, and special knitted fabrics described in JP-A-63-200467, which are sheet-like materials made of carbon fiber. Of these, carbon fiber nonwoven fabrics made of carbon fiber are more preferred in terms of handling, processability, manufacturability, etc.
[0026] When a nonwoven fabric, knitted fabric, woven fabric, or the like is used as the substrate, the average fiber length of the constituent fibers is preferably 30 to 100 mm, because a uniform carbon fiber layer can be obtained by keeping the average fiber length within this range.
[0027] The carbon fiber layer has a thickness of 1 mm or more and 5 mm or less. If the thickness is less than 1 mm, the spacer thickness must be reduced to reduce the contact resistance, which significantly deteriorates the liquid permeability within the electrode. On the other hand, if the thickness exceeds 5 mm, although the liquid permeability improves, it becomes difficult to obtain the desired resistance-lowering effect.
[0028] Nonwoven fabrics are defined in JIS L 0222, and include spunbonded nonwoven fabrics, spunlaced nonwoven fabrics, needle-punched nonwoven fabrics, resin-bonded nonwoven fabrics, and thermal-bonded nonwoven fabrics, depending on the manufacturing method, such as entanglement, fusion, or adhesion.
[0029] As described above, the carbon fiber is obtained by subjecting an organic fiber precursor to a thermal carbonization treatment, and the "thermal carbonization treatment" preferably includes at least a flame-proofing step and a carbonization (baking) step. However, the carbonization step does not necessarily have to be performed after the flame-proofing step as described above, and may be performed after impregnation of flame-proofed fibers as described in the examples below. In this case, the carbonization step after the flame-proofing step can be omitted.
[0030] Among these, the flame-resistant process refers to a process of heating an organic fiber precursor in an air atmosphere at a temperature of preferably 180°C or higher and 350°C or lower to obtain a flame-resistant organic fiber. The heat treatment temperature is more preferably 190°C or higher, and even more preferably 200°C or higher. It is also more preferably 330°C or lower, and even more preferably 300°C or lower. By heating within the above temperature range, the organic fiber does not undergo thermal decomposition, and the nitrogen and hydrogen contents in the organic fiber can be reduced while maintaining the carbon fiber form, thereby improving the carbonization rate. During the flame-resistant process, the organic fiber may thermally shrink, causing the molecular orientation to collapse and reducing the conductivity of the carbon fiber. Therefore, it is preferable to perform the flame-resistant treatment on the organic fiber under tension or stretching, and more preferably under tension.
[0031] The carbonization step refers to a step of heating the flame-resistant organic fiber obtained as described above in an inert atmosphere (preferably a nitrogen atmosphere) at a temperature of preferably 1000°C or higher and 2000°C or lower to obtain a carbon fiber. The heating temperature is more preferably 1100°C or higher, and even more preferably 1200°C or higher. Also, it is more preferably 1900°C or lower. By performing the carbonization step within the above temperature range, the carbonization of the organic fiber progresses, and carbon fiber having a pseudo-graphite crystal structure can be obtained.
[0032] Since organic fibers have different crystallinity, the heating temperature in the carbonization step can be selected depending on the type of organic fiber used as the raw material. For example, when an acrylic resin (preferably polyacrylonitrile) is used as the organic fiber, the heating temperature is preferably 800°C or higher and 2000°C or lower, and more preferably 1000°C or higher and 1800°C or lower.
[0033] The flame-proofing step and carbonization step are preferably carried out continuously, and the temperature rise rate when raising the temperature from the flame-proofing temperature to the carbonization temperature is preferably 20°C / min or less, more preferably 15°C / min or less. By setting the temperature rise rate within the above range, it is possible to obtain carbon fibers that retain the shape of the organic fibers and have excellent mechanical properties. Note that the lower limit of the temperature rise rate is preferably 5°C / min or more, taking into account the mechanical properties, etc.
[0034] [Carbonized Binder] According to the present invention, a carbon electrode material can be obtained in which the carbonized binder is unevenly distributed on both surfaces of the carbon fiber layer. Furthermore, similar to the carbonized binder, carbon particles are unevenly distributed on both surfaces of the carbon fiber layer. Hereinafter, the region consisting of a composition (carbon binder, carbon particles, etc.) attached to the carbon fibers contained in the electrode material will be referred to as the "carbonized binder-containing layer." It is preferable that part or all of the carbonized binder-containing layer is present inside the carbon fiber layer. It is preferable that the carbonized binder-containing layer is unevenly distributed on both surfaces of the carbon fiber layer. The carbon particles contained in the carbonized binder-containing layer increase the specific surface area of the carbon electrode and promote the oxidation-reduction reaction of vanadium. Furthermore, by unevenly distributing the attachment on both surfaces, sufficient voids in the carbon fiber layer can be maintained, resulting in high liquid permeability. Furthermore, the carbonized binder-containing layer unevenly distributed on the surface suppresses fluffing of the carbon fibers, thereby preventing short circuits.
[0035] Examples of methods for forming a layer containing a carbonizing binder include known methods such as applying a slurry to one side of a carbon fiber layer and drying it, applying a slurry and then laminating the dried film to the carbon fiber layer, and spray coating. In the present invention, a preferred method involves applying the slurry to a smooth film or release paper, bringing the coated surface into contact with the carbon fiber layer, and then drying to integrate them. This method allows the smoothness of the film or release paper to be transferred to the layer containing a carbonizing binder, which is preferable in terms of suppressing short circuits. Furthermore, when contacting the coated surface with the carbon fiber layer, the degree of impregnation of the slurry into the carbon fiber layer can be controlled by adjusting the coating thickness, viscosity, and pressure during contact, which is preferable in terms of ensuring an open area ratio.
[0036] The slurry contains a carbonized binder precursor, carbon particles, and organic binder components such as polyvinyl alcohol, which will be described later. The solvent used in the coating slurry can be either water or an organic solvent, but water is preferred from the standpoint of environmental impact. When water is used, it is preferable to add any known surfactant, taking into account its affinity with the carbonized binder precursor and carbon particles. In this case, it is preferable that the surfactant has a low carbon residue rate and does not contain alkali metals, transition metals, or the like.
[0037] The viscosity of the slurry is preferably 1000 to 20000 cPs. If the viscosity is lower than 1000 cPs, the coating liquid will flow due to the inclination of the substrate, making it difficult to control the coating thickness. On the other hand, if the viscosity is higher than 20000 cPs, the coating liquid will not easily penetrate into the carbon fiber layer, resulting in a significant decrease in the surface opening ratio, which is undesirable. The viscosity can be adjusted by adding a known thickener or an organic binder component such as polyvinyl alcohol.
[0038] Additives may be added to the slurry as desired, such as milled carbon fiber that can mechanically reinforce the layer containing the carbonized binder, or organic beads or piles that intentionally form voids in the layer containing the carbonized binder.
[0039] [Carbon Particles] In the present invention, "carbon particles" are useful for increasing the reaction surface area and accelerating the oxidation-reduction reaction of vanadium ions.
[0040] First, the particle size of the "carbon particles" used in the present invention is 0.001 to 20 μm, preferably 0.005 to 10 μm. If the particle size exceeds 20 μm, the reactive surface area becomes small, making it difficult to achieve a low-resistance effect. On the other hand, if the particle size is 0.001 μm or less, the proportion of particles buried in the binder increases, or in very small spaces, the electrolyte is less likely to contact due to surface tension, etc., which may reduce the proportion of particles effective for the reaction. Here, "particle size" refers to the average particle size (D50) at the median 50% diameter in the particle size distribution obtained by dynamic light scattering or other methods. In this case, even if the primary particle size is 0.01 μm or less, it is sufficient that the secondary particle size of the aggregates is 0.01 μm or more. In this way, by appropriately selecting the particle size of the carbon particles, the supported carbon particles can be effectively utilized.
[0041] The BET specific surface area calculated from the nitrogen adsorption amount of the "carbon particles" used in the present invention is 5 m 2 / g or more is preferable, and 10m 2 / g or more is more preferable, and 50m 2 / g or more is more preferable, and 100m 2 / g or more is particularly preferred, and 200m 2 / g or more is most preferable. 2If the surface area is less than 1000 m / g, the edge exposure of the carbon particles is reduced, and the contact area with the electrolyte is also reduced, making it difficult to obtain the desired low resistance. Although the upper limit is not particularly limited from the above viewpoint, in the case of particles with a large surface area and high bulk, the viscosity of the dispersion solution is likely to increase, and considering that the processability into a sheet or the like is deteriorated, it is generally set to 2000 m / g. 2 / g or less, and 2 / g or less is more preferable, and 1000m 2 The "BET specific surface area determined from the amount of nitrogen adsorption" means the specific surface area calculated from the amount of gas molecules adsorbed when nitrogen molecules are adsorbed onto solid particles.
[0042] As the "carbon particles" used in the present invention, for example, carbon blacks such as acetylene black (acetylene soot), oil black (furnace black, oil soot), ketjen black, and gas black (gas soot) are often used, which have high reactivity and specific surface area and low crystallinity. In addition to the above, carbon nanotubes (CNTs), carbon nanofibers, carbon aerogels, mesoporous carbon, graphites, graphene, graphene oxide, N-doped CNTs, boron-doped CNTs, and fullerenes are also used. From the viewpoint of raw material cost, carbon blacks are preferably used.
[0043] The content of the "carbon particles" used in the present invention is preferably 5% or more, more preferably 10% or more, in terms of mass ratio relative to the total amount of the carbon fiber, carbon particles, and carbonized binder described below. This allows the effectiveness of the supported carbon particles to be fully obtained, resulting in reduced resistance. However, if the amount of carbon particles is excessive, the layer unevenly distributed on the surface of the carbon fiber layer will clog the surface, resulting in increased resistance. Therefore, the upper limit is preferably approximately 90% or less. Note that the carbon fiber content used to calculate the above content is the content of the structure when a structure such as a carbon fiber nonwoven fabric is used as the carbon fiber layer.
[0044] In the present invention, the mass ratio of the carbonized binder (described below) to the carbon particles is preferably 0.05 to 20, more preferably 0.1 to 10, and even more preferably 0.15 to 3. If the ratio is less than 0.05, many carbon particles will fall off, and the carbon particles will not be sufficiently bound to the carbon material. On the other hand, if the ratio exceeds 20, the carbon edge surfaces of the carbon particles, which are the reaction sites, will be covered, and the desired low resistance will not be obtained.
[0045] [Carbonized Binder] The carbonized binder used in the present invention is added as a binder that is electrically conductive and that strongly binds carbon fibers and carbon particles, which are normally unable to bind together. In the present invention, by unevenly distributing layers containing not only a binder but also a carbonized binder on both surfaces of the carbon fiber layer, it is possible to maintain a state in which sufficient voids are secured in the carbon fiber layer and to achieve high liquid permeability. In addition, the layer containing the carbonized binder unevenly distributed on the surface suppresses fluffing of the carbon fibers, thereby making it possible to suppress short circuits.
[0046] The carbonized binder used in the present invention has a peak at 1360 cm determined by laser Raman spectroscopy. -1 The peak intensity of ID and 1580 cm -1 The ratio of the peak intensity I to the peak intensity I (ID / IG) is preferably 0.3 to 1.5. By using a highly crystalline carbonized binder having a crystallinity of 0.3 to 1.5, the electron conduction resistance between the carbon particles and the carbon fibers is reduced, and the electron conduction path between the carbon particles and the carbon fibers becomes smooth.
[0047] In the present invention, the ID / IG ratio of the carbonized binder is preferably 0.3 or more, more preferably 0.8 or more, in consideration of the balance of affinity with the electrolyte, while it is preferably about 1.5 or less in consideration of the electronic conductivity from the above viewpoint.
[0048] The content of the carbonized binder relative to the total amount of the carbon fibers, carbon particles, and carbonized binder is preferably 5% or more, more preferably 10% or more, and even more preferably 15% or more. By increasing the content of the carbonized binder in this way, both the carbon fibers and the carbon particles can be sufficiently bound. Note that the upper limit is preferably approximately 60% or less, taking into consideration the permeability of the electrolyte and the suppression of surface coating of the carbon particles.
[0049] The mass ratio of the total content of the carbon particles and the carbonized binder to the total amount of the carbon fibers, carbon particles other than graphite particles, and the carbonized binder is not particularly limited as long as the above requirements are satisfied, but is, for example, 20 to 65%. By setting the mass ratio in this range, both liquid permeability and low resistance can be achieved.
[0050] The type of starting material for the carbonized binder used in the present invention may be any material capable of binding carbon fibers and carbon particles, and specifically, is not particularly limited as long as it exhibits binding properties upon carbonization during the preparation of the electrode material 5 of the present invention. Examples of such materials include pitches such as coal tar pitch and coal-based pitch; resins such as phenolic resins, benzoxazine resins, epoxide resins, furan resins, vinyl ester resins, melamine-formaldehyde resins, urea-formaldehyde resins, resorcinol-formaldehyde resins, cyanate ester resins, bismaleimide resins, polyurethane resins, and polyacrylonitrile; furfuryl alcohol; and rubbers such as acrylonitrile-butadiene rubber. Commercially available products may also be used.
[0051] Among these, pitches such as coal tar pitch and coal-based pitch, which are particularly easily crystalline, are preferred because they can produce highly crystalline carbonized binders at low firing temperatures. Other resins are also preferably used because the desired carbonized binders can be obtained by increasing the firing temperature. Pitches are particularly preferred.
[0052] Here, particularly preferred pitches are described in detail. The mesophase (liquid crystal phase) content of the aforementioned coal tar pitch and coal-based pitch can be controlled by the temperature and time of the infusibility treatment. If the mesophase content is low, the pitch will melt at a relatively low temperature or will be in a liquid state at room temperature. On the other hand, if the mesophase content is high, the pitch will melt at a high temperature and a high carbonization yield will be obtained. When pitches are used as carbonization binders, it is preferable that the mesophase content is high (i.e., the carbonization rate is high), for example, 30% or more is preferred, and 50% or more is more preferred. This suppresses fluidity during melting and allows carbon fibers to be bonded together via the carbon particles without excessively coating the surfaces of carbon particles other than graphite particles. Note that the upper limit is preferably, for example, 90% or less, taking into consideration the expression of binding properties.
[0053] From the same viewpoint as above, the melting point of the pitches is preferably 80°C or higher, and more preferably 100°C or higher. This not only achieves the above-mentioned effects, but also suppresses odor during the impregnation process, which is preferable in terms of processability. Note that the upper limit is preferably 350°C or lower, for example, in consideration of the development of binding properties.
[0054] (Characteristics of the Electrode Material of the Present Invention) In the electrode material 5 of the present invention, a layer containing a carbonized binder is unevenly distributed on both surfaces of the carbon fiber layer, and the surface opening ratio determined by binarization of images obtained by electron microscopy is 30 to 50%. This can be achieved by controlling the degree of impregnation of the slurry into the carbon fiber layer by adjusting the coating amount, coating thickness, viscosity, and contact pressure when contacting the slurry-coated surface with the carbon fiber layer. According to the present invention, the carbon particles contained in the layer containing the carbonized binder increase the specific surface area of the carbon electrode and promote the oxidation-reduction reaction of vanadium. Furthermore, by unevenly distributing the additive on both surfaces, sufficient voids in the carbon fiber layer can be maintained, resulting in high liquid permeability. Furthermore, the layer containing the carbonized binder unevenly distributed on the surface suppresses fuzzing of the carbon fiber, thereby preventing short circuits. Increasing the diameter of carbon fibers to provide high liquid permeability, as in the past, has been found to increase the strength of the single fiber, dramatically increasing the risk of the carbon fiber penetrating the ion exchange membrane, making it difficult to achieve both this and short-circuit prevention. Furthermore, if the carbonized binder and carbon particles are supported throughout the carbon fiber layer, rather than being unevenly distributed on the surface, the binding action of the carbonized binder increases the strength of the single fiber, similarly increasing the risk of membrane damage. However, by intentionally unevenly distributing the layer containing the carbonized binder on the surface as in the present invention, it is believed that the aforementioned effects make it possible to achieve the desired low resistance, high liquid permeability, and short-circuit prevention.
[0055] The surface porosity described herein can be determined by image analysis, such as binarization of a microscopic image acquired by an electron microscope. Specifically, when observing the surface with a scanning electron microscope, the dark-viewed area can be considered to be voids, and the bright-viewed area can be considered to be areas occupied by the carbon electrode. The surface porosity, i.e., the ratio of dark-viewed area to bright-viewed area, can be calculated by binarizing the image using known image analysis software, with a specific brightness as a boundary. In the present invention, by ensuring a surface porosity within a specific range in the layer containing a carbonized binder unevenly distributed on the surface, it is possible to achieve low resistance and high liquid permeability while suppressing short circuits. In other words, if the surface porosity is significantly reduced, the protective effect of the layer containing the carbonized binder is enhanced, but ion conduction to the membrane is inhibited and the liquid contact efficiency of the layer containing the carbonized binder is reduced, making it impossible to simultaneously achieve low resistance and effective short-circuit suppression. On the other hand, if the surface porosity is significantly increased, the protective effect and reaction-promoting effect of the layer containing the carbonized binder are weakened, resulting in low resistance and ineffective short-circuit suppression.
[0056] The phrase "the carbonized binder-containing layer is unevenly distributed on both surfaces" refers to a state in which the carbonized binder or carbon particles are not present near the center in the thickness direction of the carbon fiber layer, but are present only on both surfaces. This can be determined from microscopic images of the cross section of the electrode material 5, such as those shown in Figures 6 and 7. When the entire cross section of the electrode material 5 is observed, layers containing the carbonized binder are clearly observed on both surfaces of the electrode material 5 of the present invention. Because the layers have openings, the observed layers do not need to be continuous.
[0057] According to the present invention, the surface opening ratio determined by binarizing a microscopic image acquired by an electron microscope is 30 to 50%, and preferably 35 to 50%. Ensuring a high surface opening ratio makes it possible to achieve low resistance and high liquid permeability while also achieving short-circuit suppression, for the reasons described above. If the surface opening ratio exceeds 50%, the protective and reaction-promoting effects of the layer containing the carbonized binder are weakened, making it impossible to achieve low resistance or effective short-circuit suppression. On the other hand, if the surface opening ratio is less than 30%, ion conduction to the membrane is inhibited and the liquid contact efficiency of the layer containing the carbonized binder is reduced, making it impossible to achieve both low resistance and high short-circuit suppression.
[0058] In order to achieve the above-mentioned opening ratio, the weight of the layer containing the carbonized binder is 30 to 90 g / m per side. 2 It is preferable that the density is 40 to 70 g / m 2 It is particularly preferable that the weight of the layer containing the carbonized binder is 30 g / m. 2 If the weight is less than 90 g / m, the desired low resistance and short circuit suppression cannot be obtained for the reasons mentioned above. 2 If the amount is more than this, ion conduction to the film is inhibited and the liquid contact efficiency of the layer containing the carbonized binder is deteriorated, so that both low resistance and low resistance cannot be achieved.
[0059] In the present invention, it is preferable that a part or all of the carbonized binder is present inside the carbon fiber layer, that is, it is preferable that a part or all of the layer containing the carbonized binder is present inside the carbon fiber layer. If the carbonized binder-containing layer is not impregnated into the carbon fiber layer at all, the bonding between the carbonized binder-containing layer and the carbon fiber layer is poor, and peeling of the carbonized binder-containing layer occurs, which is not preferable. In addition, there is a concern that the contact resistance between the carbonized binder-containing layer and the carbon fiber layer may increase.
[0060] The layer containing the carbonized binder preferably exists to a depth of 5 to 30% from both surfaces, assuming the total thickness of the carbon fiber layer to be 100%. If the layer containing the carbonized binder exists only to a depth of less than 5% from the surface, the bonding between the layer containing the carbonized binder and the carbon fiber layer may be poor, which may cause the aforementioned deterioration in quality. On the other hand, if the layer containing the carbonized binder exists to a position deeper than 30% from the surface, it may fill the voids inside the carbon fiber layer, making it difficult to achieve both liquid permeability. Note that in all of the examples described below, the layer containing the carbonized binder exists to a depth of 5 to 30% from both surfaces.
[0061] The weight of the electrode material 5 of the present invention is 100 to 700 g / m when the thickness of the spacer 2 sandwiched between the current collector plate 1 and the ion exchange membrane 3 (hereinafter referred to as "spacer thickness") is 1 to 4 mm. 2 is preferred, and 150 to 400 g / m 2By controlling the basis weight within the above range, it is possible to ensure liquid permeability while preventing excessive surface pressure from being applied to the ion exchange membrane 3, thereby reducing the risk of short-circuiting.
[0062] The thickness of the electrode material 5 of the present invention is preferably at least greater than the thickness of the spacer. For example, it is preferably 1.5 to 6.0 times the thickness of the spacer. However, if the thickness is too large, the compressive stress of the sheet-like material may break through the ion exchange membrane 3. Therefore, the compressive stress of the electrode material 5 of the present invention is set to 9.8 N / cm. 2 The following are preferably used: The electrode material 5 of the present invention can be used in a laminate of two or three layers, or can be combined with an electrode material of another form.
[0063] Each step in producing the electrode material 5 of the present invention will be described below. The production includes the following steps (1) to (6). The production method using nonwoven fabric will be described below. (1) A step of preparing a flame-resistant nonwoven fabric made of flame-resistant fibers. (2) A step of applying a paste containing a carbonized binder precursor onto a substrate, bringing the flame-resistant nonwoven fabric into contact with this, and drying. (3) A step of adjusting the thickness by heat pressing. (4) A step of carbonizing at 500 to 2000°C. (5) A step of graphitizing at 1300 to 2200°C. (6) A step of oxidizing.
[0064] (Step of Preparing a Nonwoven Fabric Made of Flame-Resistant Fibers) First, carbon fiber precursor staple fibers such as flame-resistant polyacrylonitrile, or a predetermined amount of space-forming staple fibers, are added thereto, and a nonwoven fabric can be formed by any known method. For example, the staple fibers are defibrated and then a web is produced using a carding machine. The web is then laminated in cross layers or parallel layers, and then formed into a nonwoven fabric using needle punching, calendaring, water jetting, or the like. The web may be of a single composition, or may have a layer structure of different compositions, with each layer assigned the functions of low resistance and high liquid permeability.
[0065] (Process for unevenly distributing a layer containing carbon particles and a carbonizable binder on a nonwoven fabric) Carbon particles and a carbonizable binder precursor are attached to the surface of the nonwoven fabric obtained in the nonwoven fabric formation process. To attach the carbon particles and the carbonizable binder precursor, the carbonizable binder precursor and carbon particles are dispersed in a solvent such as water or alcohol to which a binder (temporary adhesive) that disappears upon carbonization, such as polyvinyl alcohol, is added. This dispersion is then coated onto a smooth film or release paper, the coated surface is brought into contact with the nonwoven fabric, and the layers are dried to form a single unit. By performing this process on both the front and back surfaces, a layer containing the carbonizable binder can be unevenly distributed on both surfaces. Known methods such as knife coating and die coating can be used for coating, and the coating amount can be controlled by the thickness, discharge rate, etc. Furthermore, the degree of impregnation of the carbonizable binder layer into the nonwoven fabric can be controlled by changing the viscosity of the coating liquid and the load applied when contacting the coated surface with the nonwoven fabric.
[0066] Thereafter, the coated film is dried in an air atmosphere at, for example, 80 to 150°C.
[0067] (Carbonization Step) The carbonization step is performed to calcinate the product obtained after the impregnation step in the above step. This allows the carbon particles, carbon fibers, and carbonized binder to bond together. In the carbonization step, it is preferable to sufficiently remove decomposition gases generated during carbonization. For example, heating is performed in an inert atmosphere (preferably a nitrogen atmosphere) at a temperature of 500°C or higher and lower than 2000°C. The heating temperature is preferably 600°C or higher, more preferably 800°C or higher, even more preferably 900°C or higher, and particularly preferably 1000°C or higher; more preferably 1400°C or lower, even more preferably 1300°C or lower, and particularly preferably 1200°C or lower. The heating time in the inert atmosphere is preferably, for example, 1 to 2 hours. Such a short treatment time sufficiently promotes bonding between the carbon fibers and removal of decomposition gases generated during carbonization.
[0068] (Graphitization Step) The graphitization step is a step carried out to sufficiently increase the crystallinity of the carbon material, thereby improving electronic conductivity and oxidation resistance to sulfuric acid solutions in the electrolyte. The graphitization step is preferably carried out in an inert atmosphere (preferably a nitrogen atmosphere) at a temperature of 1300°C or higher, which is higher than the heating temperature in the carbonization step, and more preferably 1500°C or higher. Note that the upper limit is preferably 2200°C or lower, in consideration of imparting high affinity to the electrolyte to the carbon material.
[0069] (Oxidation Process) In the present invention, after the graphitization process, a dry oxidation process is performed to introduce oxygen functional groups, such as hydroxyl groups, carbonyl groups, quinone groups, lactone groups, and free radical oxides, onto the surface of the electrode material 5, thereby bonding oxygen atoms to carbon atoms on the surface of the electrode material. By performing the oxidation process, the ratio of the number of oxygen atoms bonded to carbon atoms on the surface of the electrode material to the total number of carbon atoms on the surface of the electrode material (hereinafter referred to as the O / C ratio) can be set to 1.0 atomic % or more. Because oxygen functional groups significantly contribute to electrode reactions, a sufficiently low resistance can be obtained by setting the O / C ratio within the above range. The O / C ratio is preferably 3 to 15 atomic %, and more preferably 5 to 10 atomic %.
[0070] Various oxidation treatment processes, such as wet chemical oxidation, electrolytic oxidation, and dry oxidation, can be applied to the oxidation treatment process. In the present invention, dry oxidation treatment is performed from the viewpoint of workability and manufacturing costs. Preferably, the oxidation treatment is performed in an air atmosphere. The heating temperature is controlled to a range of 500°C or higher and 900°C or lower. This introduces oxygen functional groups to the surface of the electrode material 5, thereby effectively achieving the above-mentioned effects. The heating temperature is preferably 600°C or higher, more preferably 650°C or higher. It is also preferably 800°C or lower, more preferably 750°C or lower. Similarly to the primary oxidation treatment described above, the oxidation treatment is preferably performed for, for example, 5 minutes to 1 hour. If the primary oxidation treatment solution is used for less than 5 minutes, there is a risk that the entire electrode material 5 will not be oxidized uniformly. On the other hand, if the primary oxidation treatment solution is used for more than 1 hour, there is a risk that the strength of the electrode material 5 will decrease, resulting in reduced productivity.
[0071] Furthermore, in the oxidation treatment step, it is preferable to adjust the mass yield of the electrode material 5 before and after the oxidation treatment (i.e., the ratio of the mass of the electrode material 5 after the secondary oxidation treatment to the mass of the electrode material 5 before the secondary oxidation treatment) to 85% or more and 96% or less, from the viewpoint of maintaining the mechanical strength of the electrode material 5. The mass yield can be adjusted, for example, by appropriately adjusting the treatment time and heating temperature of the dry air oxidation.
[0072] This application claims the benefit of priority based on Japanese Patent Application No. 2023-053421, filed on March 29, 2023. The entire content of the specification of Japanese Patent Application No. 2023-053421, filed on March 29, 2023, is incorporated herein by reference.
[0073] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to the following examples.
[0074] First, the measurement methods for the items measured in the following Examples and Comparative Examples will be described.
[0075] (1) Carbon Fiber Diameter The electrode material obtained by the method described below was cut into 5 mm squares and Au was vapor-deposited using a sputtering device. The fiber cross section of the carbon electrode material was observed under a scanning electron microscope at 3000 magnifications, and the width of the fiber observed in the field of view was measured. Similar measurements were performed at a total of 10 locations, and the average value was calculated to obtain the average fiber diameter.
[0076] (2) Surface Opening Ratio The electrode material obtained by the method described below was cut into 5 mm squares and Au was vapor-deposited using a sputtering device. It was then set on a sample stage, and both sides were photographed at 30x magnification using a scanning electron microscope TM3030Plus manufactured by Hitachi High-Technologies Corporation. The photographed image was converted to grayscale using WinROOF manufactured by Mitani Shoji Co., Ltd., and the luminance (brightness) of each pixel in the image was divided into 256 levels, with the darkest luminance being 0 and the brightest luminance being 255. Relatively bright pixels with luminances of 109 to 255 were taken as the area of the carbon electrode portion, and the surface opening ratio was calculated using the following formula 1. The average of the surface opening ratios of both sides was taken as the surface opening ratio of the electrode material. Surface opening ratio [%] = 100 - (area of carbon electrode portion / total area × 100) ... (Formula 1)
[0077] (3) BET specific surface area (BET: m 2 Approximately 50 mg of the electrode material was weighed out and vacuum dried at 130° C. for 24 hours. The amount of nitrogen adsorption was measured for the dried sample using an automatic specific surface area measuring device (Shimadzu Corporation, GEMINI VII) by a gas adsorption method using nitrogen gas, and the BET specific surface area (m 2 / g) was determined.
[0078] (4) Total Cell Resistance Each electrode material obtained by the method described below was placed in a 16 cm2 electrode area measuring 10 cm in the vertical direction (flow direction) and 1.6 cm in the width direction. 2 The cell shown in Figure 2 was assembled. The ion exchange membrane used was an APS4 membrane manufactured by Asahi Glass Co., Ltd., and the spacer thickness was 1.5 mm. 2 The total cell resistance was calculated from the voltage curve after two cycles in the voltage range of 1.70 to 1.00 V using the following formula 2. The cathode electrolyte used was a 2.5 mol / L aqueous sulfuric acid solution containing 1.7 mol / L vanadium oxysulfate, and the anode electrolyte used was a 2.5 mol / L aqueous sulfuric acid solution containing 1.7 mol / L vanadium sulfate. The electrolyte volume was 10 mL, the flow rate was 20 mL per minute, and the measurement was carried out at 30°C. The charge voltage V corresponding to the amount of electricity when the charge rate is 50% is C50 , discharge voltage V D50 are calculated from the voltage curve, and the current density is calculated as I (mA / cm 2 ) and the total cell resistance (Ω cm 2 The total cell resistance (Ω cm 2 ) = (V C50 -V D50 ) / 2I (Equation 2) where, V C50 is the value obtained from the electrode curve of the charging voltage for the amount of electricity when the charging rate is 50%, V D50 is the value obtained from the electrode curve of the discharge voltage relative to the amount of electricity when the charge rate is 50%, and (5) Liquid permeability Each electrode material obtained by the method described below was placed in an electrode with an electrode area of 16 cm, 10 cm in the vertical direction (liquid flow direction) and 1.6 cm in the width direction. 2The cell shown in Figure 2 was assembled using the electrode material. However, a 2.0 mm thick Teflon (registered trademark) sheet was used instead of the ion exchange membrane. Pure water at 25°C was pumped into the cell using a microtube pump, and the flow rate of the pure water was adjusted so that the differential pressure between the inlet and outlet was 4.9 kPa using a digital manometer, and the flow rate (mL / min) at that time was measured. (6) Basis Weight The obtained electrode material was cut into a length of 10 cm and a width of 1.6 cm, and the weight measured on a balance was used as the area (0.0016 m 2 ) was used as the basis weight. (7) Thickness A 1 cm diameter disk-shaped terminal was contacted with the obtained electrode material, and the thickness when a load of 5 gf was applied using a load cell was taken as the thickness of the electrode material. (8) Measurement of Short-Circuit Surface Pressure Two 2.5 cm square pieces were cut out of each electrode material obtained by the method described below. A Nafion 211 membrane (thickness 25 μm) was cut into a 4 cm square and sandwiched between the above-mentioned electrode material. Next, the set of the above-mentioned electrode material and Nafion 211 membrane was further sandwiched between copper plates and compressed at a rate of 0.2 mm / min using a Tensilon (RTG-1310) manufactured by A&D Company. Limited. Each copper plate used was connected to a conductor, and the DC resistance was measured with a digital multimeter. Compression was continued, and the timing at which the DC resistance of the digital multimeter was detected was taken as the short-circuit point, and the surface pressure at this time was taken as the short-circuit surface pressure (MPa). (9) Measurement of O / C by XPS surface analysis An ULVAC Phi 5801MC instrument was used for the X-ray photoelectron spectroscopy measurement. First, the sample was fixed on a sample holder with a Mo plate, and after sufficient evacuation in a preliminary evacuation chamber, it was placed in the chamber of the measurement room. Monochromated AlKα rays were used as the radiation source, with an output of 14 kV, 12 mA, and a vacuum level inside the instrument of 10. -8 Torr. A full element scan was performed to examine the composition of the surface elements, and a narrow scan was performed on the detected atoms to evaluate their abundance ratio. The ratio of the number of oxygen atoms bonded to carbon atoms on the surface of the electrode material to the total number of carbon atoms on the surface of the electrode material (O / C) was calculated as a percentage (%). The average O / C on both sides was taken as the O / C of the electrode material.
[0079] The electrode materials in the following examples and comparative examples have a specific surface area of 800 m 2 Carbon particles A, which is granular carbon black with a specific surface area of 300 m / g,2 Carbon particles B, which are granular carbon black with a fiber diameter of 21 μm, were used as the fiber substrate. Example (No. 1) First, flame-resistant polyacrylonitrile cotton with an average fiber diameter of 21 μm was defibrated with a carding machine to form a web. The obtained web was punched to a punching density of 250 holes / cm. 2 The nonwoven fabric (basis weight 250 g / m) was needle-punched. 2 , thickness 3.3 mm). Next, 2.0 mass% of a surfactant (Rheodol TW-L120 manufactured by Kao Corporation), 6.0 mass% of polyvinyl alcohol (temporary adhesive), 15 mass% of coal tar pitch (MCP100 manufactured by JFE Chemical Corporation (melting point 100°C, particle size 10 μm)), and 2.6 mass% of carbon particles A were added to ion-exchanged water, relative to 100 mass% of ion-exchanged water. Zirconia beads having a diameter of 3 mm were added to the mixture, and the mixture was subjected to a pulverization treatment using a bead mill to prepare a dispersion. The dispersion thus obtained was coated to a thickness of 500 μm on a polyester film (thickness 100 μm) manufactured by Toyobo Co., Ltd., and the flame-resistant nonwoven fabric obtained above was placed on top. A pressure of 0.01 kg / cm was applied. 2 A load of 1000 kJ / cm was applied to the sample for 1 minute, and the sample was dried on a hot plate at 80°C. After drying, the sample was peeled off from the film, and the same procedure was carried out on the other side. Next, the sample was dried at 150°C and a gauge pressure of 10 kg / cm. 2 The mixture was then heated to 1000°C at a heating rate of 5°C / min in nitrogen gas and held at this temperature for 1 hour to perform carbonization (firing). The mixture was then heated to 1500°C at a heating rate of 5°C / min in nitrogen gas and held at this temperature for 1 hour to perform graphitization. Finally, the mixture was subjected to oxidation treatment at 650°C for 5 minutes in an air atmosphere to obtain No. 1 electrode material (basis weight 225 g / m 2 The ratio of the mass after the oxidation treatment to the mass before the oxidation treatment was approximately 94%. Fig. 3 is a microscopic image of the surface of electrode material No. 1 obtained by an electron microscope. Fig. 6 is a microscopic image of the cross section of electrode material No. 1 obtained by an electron microscope.
[0080] (No. 2) An electrode material was prepared in the same manner as No. 1, except that the coating thickness of the dispersion was 250 μm. 2 , thickness 2.2 mm).
[0081] (No. 3) An electrode material No. 3 (basis weight 231 g / m) was prepared in the same manner as No. 1, except that the carbon particles used were carbon particles B. 2 , thickness 2.3 mm).
[0082] (No. 4) An electrode material No. 4 (basis weight 222 g / m) was prepared in the same manner as No. 3, except that 4% of nylon pile (fiber diameter 7 μm, fiber length 120 μm) was added to the dispersion. 2 , thickness 2.4 mm).
[0083] (No. 5) No. 5 electrode material (basis weight 230 g / m) was prepared in the same manner as No. 3, except that the oxidation treatment at 650°C was performed for 2 minutes. 2 , thickness 2.2 mm).
[0084] Comparative Example (No. 6) Felt made of flame-resistant polyacrylonitrile fibers with an average fiber diameter of 21 μm (350 g / m 2 Electrode material No. 6 (weight 220 g / m2) was prepared by carbonizing, graphitizing, and air-oxidizing the same materials as No. 1, except that the coating of the dispersion, drying operation, and heat pressing were omitted. 2 , thickness 3.6 mm).
[0085] (No. 7) The dispersion contained 9.6% MCP100 manufactured by JFE Chemical Corporation, 1.7% carbon particles A, and 2% polyvinyl alcohol. The flame-retardant nonwoven fabric was immersed in the dispersion, squeezed with nip rolls, and then dried at 120°C. The same carbonization, graphitization, and air oxidation treatments as in No. 1 were carried out to obtain No. 7 electrode material (basis weight 215 g / m). 2 Electron microscopy images of the surface of electrode material No. 7 were obtained using an electron microscope. Also, FIG. 7 is a microscopy image of the cross section of electrode material No. 7 obtained using an electron microscope.
[0086] (No. 8) An electrode material No. 8 (basis weight 409 g / m) was prepared in the same manner as No. 1, except that the content of MCP100 (melting point 100°C, particle size 10 μm) manufactured by JFE Chemical Corporation was 22%, the content of carbon particles A was 3.9%, and the coating thickness was 250 μm. 25 is a microscopic image of the surface of electrode material No. 8 obtained by an electron microscope.
[0087] (No. 9) No. 9 electrode material (basis weight 501 g / m) was prepared in the same manner as No. 8, except that the coating thickness was 500 μm. 2 , thickness 2.8 mm).
[0088] (No. 10) An electrode material No. 10 (basis weight 240 g / m) was prepared in the same manner as No. 3, except that the oxidation treatment was not performed. 2 , thickness 2.2 mm).
[0089] (No. 11) The electrode material No. 10 (basis weight 201 g / m) was prepared in the same manner as No. 3, except that the coating thickness was 250 μm and no load was applied when the nonwoven fabric was brought into contact. 2 , thickness 2.1 mm).
[0090] Table 1 shows the measurement results of various items for Nos. 1 to 11 above.
[0091]
[0092] Examples 1 to 5 are electrode materials of the present invention, and they exhibit not only low resistance and high liquid permeability, but also high short-circuit surface pressure. This is believed to be due to the mechanism described above. Specifically, the carbon particles contained in the layer containing the carbonized binder increased the specific surface area of the carbon electrode, accelerating the redox reaction of vanadium and resulting in low resistance. Furthermore, by unevenly distributing the additive on both surfaces, sufficient voids in the carbon fiber nonwoven fabric could be maintained, resulting in high liquid permeability. Furthermore, the layer containing the carbonized binder unevenly distributed on the surface suppressed fluffing of the carbon fiber, thereby preventing short circuits. When these were assembled into a cell using a Nafion 212 membrane, the current efficiency was 96%, and no decrease in efficiency due to short circuits was observed.
[0093] Comparative Example No. 6 is an example in which no carbon particles were supported. Although the liquid permeability was good, the specific surface area was low and the resistance was not low. In addition, the short-circuit surface pressure was also low.
[0094] Comparative Example No. 7 is an example in which carbon particles are supported by a carbonized binder, but are not unevenly distributed on both surfaces as in the present invention. In this case, high liquid permeability and low resistance are achieved simultaneously, but as mentioned above, the carbon fiber as a whole becomes strong due to the binding action of the carbonized binder, increasing the risk of membrane damage, and therefore the short-circuit surface pressure is low. When this example was assembled into a cell using a Nafion 212 membrane, the current efficiency was 92%, confirming the decrease in efficiency due to short-circuiting.
[0095] In Comparative Examples 8 and 9, the binder was unevenly distributed on both surfaces as in the present invention, but the surface opening ratio was low, and low resistance was not achieved. It is believed that low resistance was not achieved due to the inhibition of ion conduction to the membrane and the deterioration of liquid contact efficiency of the layer containing the carbonized binder.
[0096] Comparative Example No. 10 is an example in which the oxidation treatment was omitted and the O / C ratio was extremely low. Even with the configuration of the present invention, when the O / C ratio was extremely low, the specific surface area was not developed and low resistance was not achieved.
[0097] Comparative Example No. 11 is an example in which the carbonized binder was unevenly distributed on both surfaces as in the present invention, but no load was applied and the layer containing the carbonized binder was not impregnated. In this case, many cracks occurred in the layer containing the carbonized binder, and a large amount of the layer containing the carbonized binder fell off during handling, making it impossible to obtain an evaluable sample.
[0098] According to the present invention, it is possible to provide a carbon electrode material that not only reduces the cell resistance during initial charge and discharge but also reduces the pump load during liquid delivery and energy loss due to self-discharge, and has excellent system efficiency, and is therefore useful as an electrode material for redox batteries that use, for example, a vanadium-based electrolyte. The carbon electrode material of the present invention is suitably used in flow-type and non-flow-type redox batteries, and redox batteries combined with lithium, capacitor, and fuel cell systems.
[0099] REFERENCE SIGNS LIST 1 Current collector plate 2 Spacer 3 Ion exchange membrane 4a, 4b Liquid passage 5 Electrode material 6 Positive electrode electrolyte tank 7 Negative electrode electrolyte tank 8, 9 Pump 10 Liquid inlet 11 Liquid outlet 12, 13 External flow path
Claims
1. A carbon electrode material for redox flow batteries, characterized in that: a carbonized binder and carbon particles are unevenly distributed on both surfaces of a carbon fiber layer; the number of oxygen atoms bonded to carbon atoms on said surface is 1.0 atomic % or more of the total number of carbon atoms on said surface; a surface opening ratio determined by binarization of a microscopic image obtained by an electron microscope is 30 to 50%; and the carbon electrode material has a thickness of 1 to 5 mm.
2. The carbon electrode material according to claim 1, wherein a part or all of the carbonized binder is present inside the carbon fiber layer.
3. The carbon electrode material according to claim 1, wherein the average fiber diameter of the fibers constituting the carbon fiber layer is 10 to 30 μm.
4. A redox flow battery using the carbon electrode material according to any one of claims 1 to 3 as an electrode.
Citation Information
Patent Citations
Improved electrodes for redox flow batteries
JP2018538667A
Electrode for secondary battery and manufacturing method thereof
JP2020167078A
Carbon electrode material and redox battery
WO2020184663A1