Laminated paper tube
The paper laminate tube design addresses issues of cohesion, peeling, and bending resistance by using single-layer paper and a resin layer, achieving improved bonding and welding strength, and enhancing the paper conversion rate.
Patent Information
- Application Number
- PCT/JP2024/012343
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional paper laminate tubes face issues such as moisture-induced cohesion and peeling of the paper base layer, low paper conversion rate, insufficient bending resistance, and inadequate bonding strength when using paper as the outermost layer, as well as insufficient welding strength in flexible packaging tubes.
A paper laminate tube design featuring a sheet member with a paper base material composed of single-layer paper, a resin layer impregnated between paper layers, and a spout made of a resin material with a high MFR, along with a manufacturing method that includes bending the sheet member into a cylindrical shape and welding the spout, to enhance bonding and resistance while maintaining a high paper conversion rate.
The solution effectively suppresses agglomeration and peeling, improves bending resistance, achieves sufficient bonding strength with paper as the outermost layer, and enhances welding strength, thereby improving the overall performance and durability of the paper laminate tube.
Smart Images

Figure JP2024012343_03102024_PF_FP_ABST
Abstract
Description
Paper Laminated Tube
[0001] The present disclosure relates to a paper laminate tube, a tube container, and a method for manufacturing a paper laminate tube.
[0002] (First Background Art) For example, Japanese Patent Application Laid-Open No. 2021-104851 (Patent Document 1) describes a tube container. The tube container described in Patent Document 1 has a body portion and a head molded body. The body portion is made of a sheet member bent into a cylindrical shape. The sheet member (also referred to as sheet material) has a paper base layer. The body portion is open at one end in the longitudinal direction of the body portion and closed at the other end in the longitudinal direction of the body portion.
[0003] The head molding has a shoulder and a mouth. The shoulder is a truncated cone-shaped cylinder with an upper wall. The head molding is attached to one longitudinal end of the body at the shoulder so as to close the opening of the body. The mouth is connected to the upper wall of the shoulder. A through hole formed in the mouth communicates with the interior of the body.
[0004] The sheet member also includes a paper substrate (also referred to as paper), a barrier layer, and an adhesive layer. The adhesive layer is disposed between the paper substrate and the barrier layer, thereby adhering the barrier layer to the paper substrate. (Second Background Art) Tube containers have been proposed in the past. For example, JP 2009-532296 A (Patent Document 2) describes a package with butt-welded ends as an example of this tube container. This package includes a weldable layer forming a lower surface, a functional layer forming an upper surface, and a strip adhered to the upper surface so as to cover the end. The functional layer is made of resin, aluminum, or paper. (Third Background Art) Tube containers have been proposed in the past. For example, JP 2022-507194 A (Patent Document 3) describes a flexible cylindrical body for a packaging tube as an example of this tube container, in which two longitudinal edges of a film substrate including a plastic layer are welded to each other by a strip.
[0005] Japanese Patent Application Publication No. 2021-104851 Special Publication No. 2009-532296 Special Publication No. 2022-507194
[0006] In the tube container described in Patent Document 1, the contents are filled inside the body portion. Furthermore, the tube container described in Patent Document 1 may be exposed to external moisture.
[0007] As a first problem relating to the first background art, in the tube container described in Patent Document 1, moisture in the contents or external moisture may penetrate into the paper base layer, causing cohesive peeling of the paper base layer.
[0008] Furthermore, as a second problem related to the first background technology, the tube container described in Patent Document 1 has room for improvement in the paper content rate (the value obtained by dividing the weight of the paper base layer by the weight of the tube container and multiplying the result by 100).
[0009] A third problem related to the first background art is that in paper-laminated tubes, the stiffness of the paper substrate can make the sheet member stiff, resulting in a poor usability. To avoid this, the amount of resin material used in paper-laminated tubes is reduced. As a result, the sheet member in paper-laminated tubes can become weak against bending. To increase the sheet member's resistance to bending, it is important for the adhesive layer to penetrate into the paper substrate. In the paper-laminated tube described in Patent Document 1, the adhesive layer penetrates into the paper substrate insufficiently.
[0010] The present disclosure has been made in view of the above-described problems of the conventional art. More specifically, the present disclosure provides a paper laminated tube that can suppress cohesive peeling of the paper substrate that constitutes the body portion.
[0011] Regarding the second object, the present invention provides a paper laminated tube that can improve the paper conversion rate.
[0012] The disclosure regarding the third object has been made in view of the above-mentioned problems of the conventional art. More specifically, the present disclosure provides a paper laminate tube capable of improving the bending resistance of the sheet member.
[0013] As a fourth problem related to the second background art, there is a demand for tube containers in which the outermost layer is made of paper to create a paper-like texture. In the packaging described in the above publication, when paper is used as the outermost layer, sufficient bonding strength cannot be achieved.
[0014] The invention relating to the fourth problem was made in consideration of the above problems, and its purpose is to provide a tube container (also called a paper-laminated tube) that uses paper for the outermost layer and yet can achieve sufficient bonding strength.
[0015] As a fifth problem related to the third background art, there is a demand for tube containers made of paper to reduce the amount of plastic used. The flexible cylindrical body for packaging tubes described in the above publication cannot achieve sufficient welding strength.
[0016] The invention relating to the fifth problem has been made in view of the above problems, and its object is to provide a tube container that uses paper but can improve welding strength.
[0017] (First Means) The paper laminate tube disclosed in relation to the first object includes a body portion. The body portion is made of a sheet member having a first surface and a second surface opposite the first surface, and is bent into a cylindrical shape with the first surface facing inward. The sheet member has a paper substrate. The paper substrate includes a first single-layer paper.
[0018] In the paper laminate tube, the first monolayer paper may include a plurality of first fibers and a plurality of second fibers. The length of each of the plurality of first fibers may be longer than the length of each of the plurality of second fibers and may be 4 mm or less. The length of each of the plurality of second fibers may be 0.2 mm or more and 1.5 mm or less. The content of the first fibers in the first monolayer paper may be 50 percent or more.
[0019] In the above paper laminate tube, the basis weight of the first single layer paper is 165 g / m 2 It may be less than.
[0020] In the above-mentioned paper laminate tube, the paper substrate may further include a second single-layer paper layered on the first single-layer paper.
[0021] In the paper laminate tube, the paper substrate may further include a resin layer sandwiched between the first and second monolayer papers, and the resin layer may be impregnated into the surface of both the first and second monolayer papers.
[0022] In the above-mentioned paper laminated tube, the resin layer may be made of a resin material having a melting point of 300° C. or less.
[0023] In the above-mentioned paper laminate tube, the distance between the center of the sheet member in the thickness direction and the resin layer may be 10% or less of the thickness of the sheet member.
[0024] In the above-mentioned paper laminated tube, the sheet member, when unbent, may have a first end and a second end, which are opposite ends in a second direction perpendicular to the first direction corresponding to the longitudinal direction of the body. When the sheet member is bent into a cylindrical shape, a first surface at the first end and a second surface at the second end may be bonded. The sheet member may have a first surface resin layer on the first surface and a second surface resin layer on the second surface. The thickness of the first surface resin layer may be equal to or greater than the thickness of the second surface resin layer.
[0025] The paper-laminated tube may further include a spout having an opening communicating with the interior of the body. The spout may be made of a resin material having an MFR of 0.5 g / 10 min or more, have a maximum thickness of 2.0 mm or less, and be welded to one longitudinal end of the body. (Second Means) The paper-laminated tube disclosed regarding the first and second objects includes a body and a spout having an opening communicating with the interior of the body. The body is made of a sheet member having a first surface and a second surface opposite the first surface, and is bent into a cylindrical shape with the first surface facing inward. The sheet member has a paper base material. The spout is made of a resin material having an MFR of 0.5 g / 10 min or more, have a maximum thickness of 2.0 mm or less, and is welded to one longitudinal end of the body.
[0026] In the above-mentioned paper laminate tube, the value obtained by dividing the weight of the paper substrate by the weight of the paper laminate tube may be 50 percent or more.
[0027] The method for manufacturing a paper laminated tube disclosed in relation to the first and second problems includes the step of preparing a sheet member having a first surface and a surface opposite the first surface. The sheet member has a paper substrate. The method for manufacturing a paper laminated tube further includes the steps of bending the sheet member into a cylindrical shape with the first surface facing inward to form a body portion, forming a spout using a resin material by injection molding, and welding the spout to one longitudinal end of the body portion. (Third Means) The paper laminated tube disclosed in relation to the third problem includes a body portion. The body portion is composed of a sheet member having a first surface and a second surface opposite the first surface, and is bent into a cylindrical shape with the first surface facing inward. The sheet member includes a paper substrate, a film member, and a resin layer disposed between the paper substrate and the film member. The paper substrate is made of uncoated paper.
[0028] In the paper laminated tube, the resin layer may be impregnated to a depth of 3 μm or more from the surface of the paper substrate. In the paper laminated tube, the whiteness of the uncoated paper may be 70% or less.
[0029] In the above-mentioned paper laminated tube, the constituent material of the resin layer may be a resin material having a melting point of 300° C. or less. In the above-mentioned paper laminated tube, the constituent material of the resin layer may be a resin material having an MFR of 3 g / 10 min or more.
[0030] In the above paper laminate tube, the 10-point average roughness of the surface of the paper substrate may be 10 μm or more and 60 μm or less. (Fourth Measure) A tube container according to the invention relating to the fourth problem includes a sheet material and a tape material. The sheet material includes paper in its outermost layer and has first and second ends that are overlapped or butted together. The tape material covers the outermost layer of the sheet material to the first and second ends. The tape material includes a thermoplastic resin. The thermoplastic resin of the tape material is impregnated into the paper in the outermost layer of the sheet material. (Fifth Measure) A tube container according to the invention relating to the fifth problem includes a sheet material and a tape material. The sheet material has first and second ends that are partially overlapped and partially butted together at an angle. The tape material covers the first and second ends of the sheet material. The sheet material includes an intermediate layer, an inner layer disposed inside the intermediate layer, and an outer layer disposed outside the intermediate layer. The intermediate layer includes paper. The inner layer and the outer layer are made of a thermoplastic resin, and the tape material is welded to at least one of the inner layer and the outer layer of the sheet material.
[0031] According to the paper laminated tube disclosed regarding the first problem, it is possible to suppress cohesive peeling of the paper base material that constitutes the body portion.
[0032] According to the paper laminated tube and the method for manufacturing the paper laminated tube disclosed in relation to the second problem, it is possible to improve the paper production rate while suppressing the cohesion and peeling of the paper base material that constitutes the body portion.
[0033] According to the paper laminate tube disclosed in relation to the third problem, the bending resistance of the sheet member can be improved.
[0034] According to the tube container of the invention relating to the fourth object, sufficient bonding strength can be achieved even though paper is used for the outermost layer.
[0035] According to the tube container of the invention relating to the fifth object, it is possible to improve the welding strength while using paper.
[0036] 1. A front view of a paper laminated tube 100. A plan view of the paper laminated tube 100. A schematic cross-sectional view taken along III-III in FIG. 1. A schematic cross-sectional view taken along IV-IV in FIG. 2. A plan view of a sheet member 20 included in the paper laminated tube 100. A cross-sectional view taken along VI-VI in FIG. 5. A partial enlarged view of FIG. 3 in the vicinity of the first end 20c and the second end 20d. A partial enlarged view of FIG. 4 in the vicinity of the opening 10a. A cross-sectional view of a sheet member 20 according to a modified example. A manufacturing process diagram of a paper laminated tube. A schematic partial enlarged view of a paper laminated tube 200 in the vicinity of the opening 10a. A cross-sectional view of the second embodiment taken along VI-VI in FIG. 5. A front view schematically illustrating the configuration of a tube container according to a third embodiment. An end view schematically illustrating the configuration along line XIV-XIV in FIG. 13. An enlarged view of part XV in FIG. 14. 18 is an end view schematically showing the configuration of a first modified example of the tube container according to embodiment 3. FIG. 19 is an end view schematically showing the configuration of a second modified example of the tube container according to embodiment 3. FIG. 19 is an end view schematically showing the configuration along line XIV-XIV in FIG. 13 according to embodiment 4. FIG. 19 is an enlarged view of part XIV in FIG. 18. FIG. 20 is an end view schematically showing the configuration of a modified example of the tube container according to embodiment 4.
[0037] (Embodiment 1) Details of an embodiment of the present disclosure will be described with reference to the drawings. In the following drawings, the same or corresponding parts are designated by the same reference numerals, and redundant description will not be repeated. The paper laminate tube according to the embodiment is referred to as a paper laminate tube 100.
[0038] (Configuration of Paper Laminated Tube 100) The configuration of the paper laminated tube 100 will be described below.
[0039] Fig. 1 is a front view of the paper laminated tube 100. Fig. 2 is a plan view of the paper laminated tube 100. Fig. 3 is a schematic cross-sectional view taken along line III-III in Fig. 1. Fig. 4 is a schematic cross-sectional view taken along line IV-IV in Fig. 2. As shown in Figs. 1 to 4, the paper laminated tube 100 has a body 10, a spout 30, and a cap 40.
[0040] The paper-based rate of the paper laminated tube 100 (the weight of the paper substrate 21 described below divided by the weight of the paper laminated tube 100 multiplied by 100) is preferably 50 percent or more. When calculating the paper-based rate of the paper laminated tube 100, the weight of the paper laminated tube 100 does not include the weight of the cap 40.
[0041] The body portion 10 is formed by bending a sheet member 20 into a cylindrical shape. FIG. 5 is a plan view of the sheet member 20. FIG. 6 is a cross-sectional view taken along line VI-VI in FIG. 5. As shown in FIGS. 5 and 6, the sheet member 20 is sheet-shaped. The sheet member 20 has a first surface 20a and a second surface 20b. The first surface 20a and the second surface 20b are end surfaces of the sheet member 20 in the thickness direction. The first surface 20a faces the inside of the body portion 10 when bent into a cylindrical shape. The second surface 20b is the surface opposite to the first surface 20a. That is, the second surface 20b faces the outside of the body portion 10 when bent into a cylindrical shape.
[0042] The paper content of the body 10 (the weight of the paper base material 21 divided by the weight of the body 10 multiplied by 100) is preferably 50% or more, and more preferably 75% or more.
[0043] The sheet member 20 has a paper substrate 21. The paper substrate 21 is, for example, made of a single-ply paper 21a. The single-ply paper 21a preferably includes a plurality of first fibers and a plurality of second fibers. The length of each of the plurality of first fibers is longer than the length of each of the plurality of second fibers. The length of each of the plurality of first fibers is preferably 4 mm or less. The length of each of the plurality of second fibers is preferably 0.2 mm or more and 1.5 mm or less.
[0044] The paper base material 21 may be made of multi-layer paper, that is, the type of paper that constitutes the paper base material 21 is not particularly limited.
[0045] The content of the plurality of first fibers in the single-layer paper 21a is preferably 50 percent or more. The content of the plurality of first fibers in the single-layer paper 21a is the value obtained by dividing the number of the plurality of first fibers contained in the single-layer paper 21a by the total number of fibers contained in the single-layer paper 21a. The lengths of the first fibers and the second fibers are calculated based on an automatic optical measurement method specified in JAPAN TAPPI Paper and Pulp Testing Method No. 52 (Testing Method for Fiber Length of Paper and Pulp).
[0046] The basis weight of the single-ply paper 21a is 165 g / m 2 It is preferable that the density is less than 150 g / m 2 The basis weight of the single-ply paper 21a is measured in accordance with the method for measuring the basis weight of paper specified in the JIS standard (JIS P 8124:2011).
[0047] The sheet member 20 may further have a first surface resin layer 22 and a second surface resin layer 23. The first surface resin layer 22 constitutes the first surface 20a. The thickness of the first surface resin layer 22 is defined as thickness T1. The second surface resin layer 23 constitutes the second surface 20b. The thickness of the second surface resin layer 23 is defined as thickness T2. It is preferable that thickness T1 be greater than thickness T2. The resin material constituting the first surface resin layer 22 and the second surface resin layer 23 is, for example, polyethylene (PE). However, the resin material constituting the first surface resin layer 22 and the second surface resin layer 23 is not limited to this.
[0048] The sheet member 20 may further have a barrier layer 24, a first adhesive layer 25, and a second adhesive layer 26. The barrier layer 24 is disposed between the paper base material 21 and the first surface resin layer 22. The first adhesive layer 25 is disposed between the paper base material 21 and the barrier layer 24, and the second adhesive layer 26 is disposed between the barrier layer 24 and the first surface resin layer 22.
[0049] The barrier layer 24 is made of, for example, aluminum. More specific examples of the barrier layer 24 include one or more of the following materials: vapor deposition of a metal such as aluminum; vapor deposition of an inorganic compound such as silica or alumina; and a barrier resin coating made of a plate-like mineral and a binder resin, the barrier resin coating containing, as a component, ethylene vinyl alcohol copolymer (EVOH) or polyvinylidene chloride (PVDC). These materials may also be used in combination.
[0050] The constituent material of the first adhesive layer 25 is, for example, ethylene-methacrylic acid copolymer (EMAA). For example, the composition of the first adhesive layer 25 includes a thermoplastic resin. More specifically, the composition includes one or more of various hot melt materials such as polyolefin, polyacrylic acid, PE-based, and PP-based. There are no particular limitations on the composition of the first adhesive layer 25 as long as it can be heat-sealed to the second adhesive layer 26.
[0051] However, it is preferable to use the same material as the second adhesive layer 26, as this will increase the adhesive strength. Furthermore, the above-mentioned thermoplastic resin may be melted and bonded by extruder lamination.
[0052] Alternatively, the adhesive layer may be formed by dry lamination using an adhesive for dry lamination, such as a two-component curing urethane adhesive.
[0053] Although it has been explained that the constituent material of the second adhesive layer 26 may be the same as that of the first adhesive layer 25, a different material may also be selected as appropriate.
[0054] The constituent material of the barrier layer 24 is not limited to the above. For example, when the constituent material of the barrier layer 24 is ethylene-vinyl alcohol copolymer (EVOH), the constituent material of the first adhesive layer 25 may be polyethylene, and the second adhesive layer 26 may be omitted.
[0055] In a plan view, the first direction DR1 corresponds to the longitudinal direction of the body portion 10 when the sheet member 20 is bent. The second direction DR2 is a direction perpendicular to the first direction DR1 in a plan view. The sheet member 20 has a first end 20c and a second end 20d in the second direction DR2. The second end 20d is the end opposite the first end 20c. The sheet member 20 is bent into a cylindrical shape so that the first surface 20a faces the inside of the body portion 10, and the first end 20c and the second end 20d are bonded to each other to form the body portion 10. The bonding of the first end 20c and the second end 20d is performed, for example, by applying pressure and heat to the first end 20c and the second end 20d in an overlapping state.
[0056] 7 is a partial enlarged view of the vicinity of the first end 20c and the second end 20d of FIG. 3. As shown in FIG. 7, the side surface of the paper substrate 21 at the first end 20c and the side surface of the paper substrate 21 at the second end 20d are covered with a resin layer 27. The resin layer 27 is formed by melt-mixing the resin material constituting the first surface resin layer 22 and the resin material constituting the second surface resin layer 23.
[0057] The body portion 10 has an opening 10a at one end in the longitudinal direction of the body portion 10. The other end in the longitudinal direction of the body portion 10 is closed.
[0058] The spout 30 is attached to one longitudinal end of the body 10 so as to close the opening 10a. The spout 30 is attached by welding. The spout 30 is made of a resin material. The spout 30 is preferably formed by injection molding. That is, it is preferable that the resin material making up the spout 30 has a melt flow rate (MFR) of 0.5 g / 10 min or more and a maximum thickness of the spout 30 of 2.0 mm or less. If these conditions are not met, it may be difficult to form the spout 30 by injection molding. The MFR of the resin material making up the spout 30 is measured according to the test method defined in the JIS standard (JIS K 7210:2014).
[0059] The resin material constituting the spout 30 may have an MFR of, for example, 40 g / 10 min or less. The maximum thickness of the spout 30 may be, for example, 1.5 mm or less. The minimum thickness of the spout 30 is, for example, 0.2 mm or more.
[0060] The average thickness of the spout 30 is preferably 1 mm or less. The weight of the spout 30 is preferably 2 g or less, and more preferably 1 g or less.
[0061] The spout 30 has a protrusion 31. A thread groove (not shown) is formed on the outer peripheral surface of the protrusion 31. The thread groove of the protrusion 31 is screwed into a thread groove (not shown) formed in the cap 40, thereby removably attaching the cap 40 to the spout 30. The protrusion 31 has an opening 31a. The opening 31a communicates with the interior of the body 10. Therefore, by compressing the body 10, the contents filled inside the body 10 are dispensed from the opening 31a.
[0062] Figure 8 is a partially enlarged view of Figure 4 in the vicinity of the opening 10a. As shown in Figure 8, the spout 30 is welded to the body 10 by a resin layer 28. The resin layer 28 is formed from the same resin material as the resin material constituting the spout 30. The resin material constituting the resin layer 28 may be melt-mixed with the resin material constituting the first outer resin layer 22 and / or the resin material constituting the second outer resin layer 23. The resin layer 28 covers the side surface of the paper substrate 21 at the opening 10a.
[0063] <Modification> Figure 9 is a cross-sectional view of a sheet member 20 according to a modification. As shown in Figure 9, the paper base material 21 may have a single-layer paper sheet 21b in addition to the single-layer paper sheet 21a. The single-layer paper sheet 21b may be the same as the single-layer paper sheet 21a, or may be a different single-layer paper sheet from the single-layer paper sheet 21a. The single-layer paper sheets 21a and 21b are stacked in the thickness direction of the paper base material 21.
[0064] The paper substrate 21 may further include a resin layer 21c. The resin layer 21c is sandwiched between the single-layer paper sheets 21a and 21b, thereby bonding the single-layer paper sheets 21a and 21b together. The resin layer 21c is impregnated into the surface of the single-layer paper sheets 21a (the surface of the single-layer paper sheets 21a facing the single-layer paper sheets 21b) and into the surface of the single-layer paper sheets 21b (the surface of the single-layer paper sheets 21b facing the single-layer paper sheets 21a). The resin layer 21c is preferably impregnated to a depth of 3 μm or more from the surface of the single-layer paper sheets 21a (21b), and more preferably to a depth of 5 μm or more from the surface of the single-layer paper sheets 21a (21b).
[0065] The melting point of the resin material constituting the resin layer 21c is, for example, 300°C or less. The melting point of the resin material constituting the resin layer 21c may be 200°C or less. Specific examples of the resin material constituting the resin layer 21c include olefins, esters, etc. The thickness of the sheet member 20 is defined as thickness T. The distance between the center of the sheet member 20 in the thickness direction (see the front line in Figure 9) and the resin layer 21c is defined as distance DIS. It is preferable that distance DIS be 10 percent or less of thickness T.
[0066] (Method of Manufacturing the Paper Laminated Tube 100) A method of manufacturing the paper laminated tube 100 will be described below.
[0067] 10 is a manufacturing process diagram of a paper laminated tube. As shown in FIG. 10, the manufacturing method of a paper laminated tube 100 includes a body forming step S1, a spout forming step S2, and a spout welding step S3.
[0068] In the body portion forming step S1, first, the sheet member 20 is prepared. Second, the sheet member 20 is bent into a cylindrical shape so that the first surface 20a faces the inside of the body portion 10, and then the first end portion 20c and the second end portion 20d are overlapped with each other. Third, the first end portion 20c and the second end portion 20d are heated while being pressurized in the overlapped state. This causes the first end portion 20c and the second end portion 20d to be welded to each other. This forms the body portion 10. Thereafter, the other end portion of the body portion 10 in the longitudinal direction is welded, thereby closing the other end portion of the body portion 10 in the longitudinal direction.
[0069] In the spout forming process S2, the spout 30 is formed. The spout 30 is formed by injection molding. In the spout welding process S3, the spout 30 is attached to the body 10 by welding. More specifically, the end of the spout 30 and the end of the sheet member 20 at the opening 10a are overlapped and heated while being pressurized. This welds the end of the spout 30 and the end of the sheet member 20 at the opening 10a to each other. In this way, the paper laminate tube 100 having the structure shown in Figures 1 to 8 is formed.
[0070] (Effects of the Paper Laminated Tube 100) The effects of the paper laminated tube 100 will be described below.
[0071] Because paper is hydrogen-bonded in the planar direction (the direction perpendicular to the thickness direction of the paper), the bonding strength in the planar direction is strong. On the other hand, because paper is bonded in the thickness direction by pulp entanglement and intermolecular forces due to additives (e.g., sizing agents, paper strength improvers, etc.), the bonding strength in the thickness direction is weaker than the bonding strength in the planar direction. Therefore, when the paper base material 21 is composed of multi-layer paper, the paper base material 21 is likely to coagulate and peel when moisture penetrates into the paper base material 21.
[0072] On the other hand, in the paper laminated tube 100, the paper base material 21 is made of single-layer paper 21a. The entanglement of fibers contained in the single-layer paper 21a increases the bonding strength in the thickness direction. Therefore, the paper laminated tube 100, in which the paper base material 21 is made of single-layer paper 21a, can suppress the occurrence of cohesion and peeling when moisture penetrates the paper base material 21, compared to a paper base material 21 made of multi-layer paper. Paper laminated tubes are repeatedly squeezed to extract their contents. During this process, peeling occurs between the layers of the paper base material, degrading the functionality (rigidity, etc.) of the paper laminated tube. In the paper laminated tube 100, because the paper base material 21 is made of single-layer paper 21a, peeling between the layers of the paper base material 21 is less likely to occur, and the functionality of the paper laminated tube 100 is less likely to deteriorate even when the above-mentioned process is repeated.
[0073] (Effects of the Paper Laminated Tube 100 Compared with Comparative Examples) The effects of the paper laminated tube 100 will be described below in comparison with comparative examples.
[0074] The paper laminated tube according to the comparative example is referred to as the paper laminated tube 200. The configuration of the paper laminated tube 200 is the same as that of the paper laminated tube 100, except that the MFR of the resin material constituting the spout 30 is less than 0.5 g / 10 min. Figure 11 is a schematic partial enlarged view of the paper laminated tube 200 near the opening 10 a. As shown in Figure 11, when the MFR of the resin material constituting the spout 30 is less than 0.5 g / 10 min, the resin layer 28 may not flow sufficiently, and the resin layer 28 may not cover the side surface of the paper substrate 21 at the opening 10 a.
[0075] In contrast, in the paper laminated tube 100, the resin material constituting the spout has an MFR of 0.5 g / 10 min or more. The higher the MFR of the resin material constituting the spout 30, the higher the fluidity of the resin material when melted, making it easier for the resin layer 28 to cover the side surface of the paper substrate 21 at the opening 10 a. When the resin layer 28 covers the side surface of the paper substrate 21 at the opening 10 a, moisture is less likely to penetrate into the interior of the paper substrate 21 from the side surface, suppressing the occurrence of cohesion and peeling due to moisture penetration into the interior of the paper substrate 21. When the maximum thickness of the resin material constituting the spout 30 is reduced, the weight of the resin material used in the spout 30 is reduced, making it possible to increase the paper conversion rate of the paper laminated tube 100.
[0076] Because paper is hydrogen-bonded in the planar direction (the direction perpendicular to the thickness direction of the paper), the bonding strength in the planar direction is strong. On the other hand, because paper is bonded in the thickness direction by van der Waals forces, the bonding strength in the thickness direction is weak. Therefore, when the paper base material 21 is made of multi-layer paper, the paper base material 21 is likely to cohere and peel when moisture penetrates into the paper base material 21.
[0077] On the other hand, when the paper base material 21 is made of single-layer paper 21a, the entanglement of the fibers contained in the single-layer paper 21a increases the bonding strength in the thickness direction. Therefore, when the paper base material 21 is made of single-layer paper 21a, it is possible to further suppress the occurrence of cohesion and peeling when moisture penetrates into the paper base material 21, compared to when the paper base material 21 is made of multi-layer paper.
[0078] The higher the content of long fibers in the single-ply paper 21a, the more likely the fibers are to become entangled. Therefore, when the content of first fibers in the single-ply paper 21a is 50 percent or more, the bonding strength in the thickness direction of the single-ply paper 21a is further increased, further suppressing the occurrence of cohesive peeling when moisture penetrates into the paper base material 21. Furthermore, since the greater the basis weight of the paper, the more likely cohesive peeling occurs, when the basis weight of the single-ply paper 21a is 165 g / m 2 less than 150 g / m 2By making it less than this, the occurrence of cohesion and peeling when moisture penetrates into the paper substrate 21 can be further suppressed.
[0079] The thicker the single-layer paper 21a, the higher the paper yield of the body 10. However, as the thickness increases, even the single-layer paper 21a is more susceptible to cohesive peeling. Therefore, by ensuring the thickness of the paper base material 21 by stacking the single-layer paper 21a and the single-layer paper 21b, the paper yield of the body 10 can be increased while suppressing the occurrence of cohesive peeling when moisture penetrates into the paper base material 21.
[0080] When a resin layer 21c is sandwiched between the single-layer paper sheets 21a and 21b and the resin layer 21c is impregnated into the surfaces of the single-layer paper sheets 21a and 21b, the resin layer 21c improves the adhesion between the single-layer paper sheets 21a and 21b. In particular, when the melting point of the resin material constituting the resin layer 21c is 300°C or lower, the resin layer 21c is more likely to impregnate the surfaces of the single-layer paper sheets 21a and 21b, further improving the adhesion between the single-layer paper sheets 21a and 21b.
[0081] Because sheet member 20 is bent to form body 10, bending stress acts between the layers that make up sheet member 20. When distance DIS is 10% or less of thickness T, the distance from the neutral axis of bent sheet member 20 to the boundary between single-layer paper 21a and single-layer paper 21b becomes small, making it difficult for the bending stress to act on the boundary. Therefore, in this case, it is possible to suppress delamination between single-layer paper 21a and single-layer paper 21b.
[0082] When thickness T1 is greater than thickness T2, the side surface of the paper substrate 21 at the first end 20c and the side surface of the paper substrate 21 at the second end 20d are more likely to be covered by the resin layer 27. When the side surface of the paper substrate 21 at the first end 20c and the side surface of the paper substrate 21 at the second end 20d are covered by the resin layer 27, moisture is less likely to penetrate into the paper substrate 21 from the side surface, and the occurrence of cohesion and peeling due to moisture penetrating into the paper substrate 21 is further suppressed.
[0083] The greater the MFR of the resin material constituting the spout 30, the greater the fluidity of the resin material when melted, making it easier for the resin layer 28 to cover the side surface of the paper substrate 21 at the opening 10a. When the resin layer 28 covers the side surface of the paper substrate 21 at the opening 10a, moisture is less likely to penetrate into the interior of the paper substrate 21 from the side surface, further suppressing the occurrence of cohesion and peeling due to moisture penetration into the interior of the paper substrate 21. Reducing the maximum thickness of the resin material constituting the spout 30 reduces the mass of the resin material used in the spout 30, making it possible to increase the paper conversion rate of the paper laminate tube 100 (the proportion of the mass of the paper substrate 21 in the mass of the paper laminate tube 100). (Embodiment 2) Figure 12 is a cross-sectional view taken along line VI-VI in Figure 5 according to embodiment 2. As shown in Figures 5 and 12, the sheet member 20 is sheet-shaped. 12 , the sheet member 20 has a first surface 120a and a second surface 120b. The first surface 120a and the second surface 120b are end surfaces of the sheet member 20 in the thickness direction. The first surface 120a faces the inside of the body portion 10 when bent into a cylindrical shape. The second surface 120b is the surface opposite to the first surface 120a. That is, the second surface 120b faces the outside of the body portion 10 when bent into a cylindrical shape.
[0084] The sheet member 20 has a paper base material 121, sealant layers 122 and 123, a film member 124, and a resin layer 125. The paper base material 121 is made of uncoated paper. The paper base material 121 has a first surface 121a and a second surface 121b. The first surface 121a and the second surface 121b are end surfaces in the thickness direction of the paper base material 121. The second surface 121b is the surface opposite the first surface 121a. The uncoated paper has fibers protruding from the first surface 121a and the second surface 121b, and is paper that is not coated with natural minerals on the first surface 121a and the second surface 121b.
[0085] The whiteness of the paper substrate 121 is preferably 70 or less. The whiteness of the paper is measured according to the method specified in the JIS standard (JIS P 8148). The ten-point average roughness (RzJIS) of the surface (first surface 121a, second surface 121b) of the paper substrate 121 is preferably 10 μm or more and 60 μm or less. The ten-point average roughness of the surface of the paper substrate 121 is measured according to the method specified in the JIS standard (JIS B 0601).
[0086] The sealant layer 122 constitutes the first surface 120a. The sealant layer 123 constitutes the second surface 120b. The sealant layer 123 is disposed on the second surface 121b. The sealant layers 122 and 123 are made of a resin material. The sealant layers 122 and 123 are made of, for example, polyethylene (PE) or polypropylene (PP). The material of the sealant layer 122 may be the same as or different from the material of the sealant layer 123.
[0087] The film member 24 is disposed between the paper substrate 121 and the first surface 120a (sealant layer 122). The film member 124 is preferably made of a resin material. The film member 124 is preferably a barrier film. Note that even if an inorganic material is vapor-deposited on the surface of the film member 124, the film member 124 is considered to be made of a resin material. The film member 124 is, for example, a transparent barrier film whose base material is polyethylene terephthalate (PET) and on which an inorganic material is coated.
[0088] The resin layer 125 is sandwiched between the paper substrate 121 and the film member 124. This allows the film member 124 to be adhered to the first surface 121a. The film member 124 is attached in a state where the constituent material of the resin layer 125 is supplied molten onto the first surface 121a. That is, the film member 124 is extrusion laminated to the paper substrate 121. The constituent material of the resin layer 125 is, for example, polyethylene. However, the constituent material of the resin layer 125 is not limited to this. The resin layer 125 is impregnated into the first surface 121a. The resin layer 125 is preferably impregnated to a depth of 3 μm or more from the first surface 121a, more preferably to a depth of 5 μm or more from the first surface 121a, and particularly preferably to a depth of 10 μm or more from the first surface 121a.
[0089] The melting point of the resin material constituting the resin layer 125 is preferably 300° C. or less. The melting point of the resin material constituting the resin layer 125 may be 250° C. or less or 200° C. or less. The melting point of the resin material constituting the resin layer 125 is, for example, 100° C. or more. The melting point of the resin material constituting the resin layer 125 is measured by DSC (Differential Scanning Calorimetry) as defined in the JIS standard (JIS K 7123).
[0090] The MFR (Melt Flow Rate) of the resin material constituting the resin layer 125 is preferably 3 cg / 10 min or more. The MFR of the resin material constituting the resin layer 125 is more preferably 40 g / 10 min or less. The MFR of the resin material constituting the resin layer 125 is measured in accordance with the test method defined in the JIS standard (JIS K 7210).
[0091] In a plan view, the first direction DR1 corresponds to the longitudinal direction of the body 10 when the sheet member 20 is bent. The second direction DR2 is a direction perpendicular to the first direction DR1 in a plan view. The sheet member 20 has a first end 20c and a second end 20d in the second direction DR2. The second end 20d is the end opposite the first end 20c. The body 10 is formed by bending the sheet member 20 into a cylindrical shape so that the first surface 20a (120a) faces the inside of the body 10, and then bonding the first end 20c and the second end 20d to each other.
[0092] The first end 20c and the second end 20d are bonded together by, for example, applying pressure and heat to the first end 20c and the second end 20d in an overlapping state. However, the method for bonding the first end 20c and the second end 20d is not limited to this. The first end 20c and the second end 20d may be butted against each other, and an adhesive tape may be applied to the first surface 20a (120a) so as to straddle the first end 20c and the second end 20d, and an adhesive tape may be applied to the second surface 120b so as to straddle the first end 20c and the second end 20d.
[0093] The body 10 has an opening 10a at one end in the longitudinal direction of the body 10. The other end in the longitudinal direction of the body 10 is closed. The spout 30 is attached to one end in the longitudinal direction of the body 10 so as to close the opening 10a. The spout 30 is attached by welding. The constituent material of the spout 30 is a resin material.
[0094] The spout 30 has a protrusion 31. A thread groove (not shown) is formed on the outer peripheral surface of the protrusion 31. The thread groove of the protrusion 31 is screwed into a thread groove (not shown) formed in the cap 40, thereby removably attaching the cap 40 to the spout 30. The protrusion 31 has an opening 31a. The opening 31a communicates with the interior of the body 10. Therefore, by compressing the body 10, the contents filled inside the body 10 are dispensed from the opening 31a.
[0095] (Effects of the Paper Laminated Tube 100) The effects of the paper laminated tube 100 will be described below in comparison with a paper laminated tube according to a comparative example. The configuration of the paper laminated tube according to the comparative example is the same as the configuration of the paper laminated tube 100, except that the paper base material 21 is made of coated paper.
[0096] In the paper laminated tube according to the comparative example, the film member 124 is also bonded to the paper base material 121 (first surface 121a) by the resin layer 125. However, in the paper laminated tube according to the comparative example, the paper base material 121 is made of coated paper, and the surface of the coated paper is coated with natural minerals, making it difficult for the resin layer 125 to penetrate into the first surface 121a. As a result, in the paper laminated tube according to the comparative example, there is a risk that the resistance to bending of the sheet member 20 will be insufficient.
[0097] On the other hand, in the paper laminated tube 100, the paper base material 121 is made of uncoated paper, so the resin layer 125 is easily impregnated into the first surface 121a. Therefore, in the paper laminated tube 100, the paper base material 121 is made of uncoated paper, which improves the bending resistance of the sheet member 20.
[0098] In the paper laminated tube 100, the resin layer 125 is impregnated to a depth of 3 μm or more from the first surface 121a, which further improves the resistance of the sheet member 20 to bending.
[0099] The lower the melting point of the resin material constituting the resin layer 125, the more easily the resin layer 125 will be impregnated into the first surface 121a. Furthermore, the higher the MFR of the resin material constituting the resin layer 125, the more easily the resin layer 125 will be impregnated into the first surface 121a. Therefore, when the melting point of the resin material constituting the resin layer 125 is 300°C or lower and / or the MFR of the resin material constituting the resin layer 125 is 3 g / 10 min or higher, the resin material constituting the resin layer 125 will be more easily impregnated into the first surface 121a, and the resistance of the sheet member 20 to bending will be further improved.
[0100] <Bending Test> To conduct the bending test, Samples 1 to 3 were prepared as samples of the sheet member 20. In Samples 1 to 3, the whiteness and 10-point average roughness of the paper substrate 121 were changed. In Samples 1 to 3, the arithmetic mean height (Ra) and maximum height (Rz) of the surface of the paper substrate 121 were also changed. In Samples 1 and 2, the paper substrate 21 was uncoated paper, but in Sample 3, the paper substrate 121 was coated paper.
[0101] In the bending test, the folding strength of each sample is measured. First, a 15 mm wide test piece is cut from each sample. Second, the cut test piece is bent 270° in its MD (machine direction) (i.e., the direction of travel of the paper machine) with a tensile load of 10 N. This bending is repeated. If the test piece can be bent 300 times or more before breaking, the folding strength of the raw sheet is evaluated as "A." If the test piece can be bent 200 times or more but less than 300 times before breaking, the folding strength of the raw sheet is evaluated as "B." If the test piece breaks before 100 bending repetitions, the folding strength of the raw sheet is evaluated as "C." Details of each sample and the results of the bending test are shown in Table 1.
[0102]
[0103] As shown in Table 1, Samples 1 and 2 were rated B or higher in raw sheet folding endurance strength. Sample 3 was rated C in raw sheet folding endurance strength. Samples 1 and 2 had a penetration depth of 3 μm or higher. Sample 3 had a penetration depth of less than 3 μm. This shows that by using uncoated paper for the paper base material 121, the resin layer 125 can more easily penetrate into the paper base material 121, thereby increasing the raw sheet folding endurance strength of the sheet member 20 (improving the resistance to bending of the sheet member 20).
[0104] Furthermore, Sample 2 was evaluated as having a higher web folding strength than Sample 1. The whiteness of the paper substrate 121 in Sample 2 was 70 or less, while the whiteness of the paper substrate 121 in Sample 1 was greater than 70. Furthermore, the 10-point average roughness of the surface of the paper substrate 121 in Sample 2 was 10 μm or more and 60 μm or less, while the 10-point average roughness of the surface of the paper substrate 121 in Sample 1 was not within the range of 10 μm or more and 60 μm or less. This comparison demonstrates that the web folding strength of the sheet member 20 is further increased (the bending resistance of the sheet member 20 is further improved) by setting the whiteness of the paper substrate 121 to 70 or less or setting the 10-point average roughness of the surface of the paper substrate 121 to 10 μm or more and 60 μm or less. (Embodiment 3) The configuration of a tube container 300 according to embodiment 3 will be described with reference to FIG. 13 . The tube container 300 according to this embodiment includes a body portion 201 and a pouring portion 202.
[0105] The body 201 is a member for accommodating the contents. The body 201 is configured in a tubular shape. The body 201 is configured by molding a sheet material 210 having a pair of approximately parallel edges into a tubular shape. A rear end 201a of the body 201 is closed by heat sealing. A front end 1b of the body 201 is welded to the pouring portion 202.
[0106] The spout 202 is a member for pouring the contents contained in the body 201 to the outside. The spout 202 includes a mouth 202a and a flange 202b. The mouth 202a is configured in a cylindrical shape. The flange 202b is connected to the rear end of the mouth 202a. The flange 202b is configured to protrude outward from the mouth 202a. The outer shape of the flange 202b is configured in a truncated cone shape.
[0107] The tube container 300 may further include a cap 203. The cap 203 is configured to be detachable from the dispensing part 202. The cap 203 may be a screw cap that can be detachably attached to the opening 202a of the dispensing part 202 by screwing it onto the opening 202a.
[0108] 13 and 14 , the tube container 300 includes a sheet material 210 and a tape material 220. The sheet material 210 includes a first end E201 and a second end E202 that are overlapped or abutted against each other. In this embodiment, the sheet material 210 includes the first end E201 and the second end E202 that are overlapped with each other. Specifically, the first end E201 covers the second end E202 from the outside. The first end E201 is one end in the width direction of the sheet material 210, and the second end E202 is the other end in the width direction of the sheet material 210. The first end E201 is a first end that is a region that has a width toward the second end E202. The second end E202 is a second end that is a region that has a width toward the first end E201.
[0109] The tape material 220 covers the first end E201 and the second end E202 from the outermost layer of the sheet material 210. The tape material 220 covers a portion of the outer surface of the sheet material 210. The tape material 220 may cover the first end E201 and the second end E202 continuously from the leading end to the trailing end of the sheet material 210 in the length direction perpendicular to the width direction of the sheet material 210.
[0110] 14 and 15 , sheet material 210 includes paper in an outermost layer 211. Tape material 220 includes thermoplastic resin. The thermoplastic resin of tape material 220 is impregnated into the paper of the outermost layer of sheet material 210.
[0111] The configuration of the sheet material 210 of this embodiment will be described in detail. In this embodiment, the sheet material 210 includes an outermost layer 211, an intermediate layer 212, and an innermost layer 213. The outermost layer 211, the intermediate layer 212, and the innermost layer 213 are laminated in this order from the outside.
[0112] In the region where the first end E201 and the second end E202 overlap each other, the outermost layer 211 of the first end E201 overlaps the outer surface of the outermost layer 211 of the second end E202. In the region where the first end E201 and the second end E202 overlap each other, the innermost layer 213 of the second end E202 overlaps the inner surface of the innermost layer 213 of the first end E201.
[0113] Between the overlapping regions of the first end E201 and the second end E202, there is provided a region where the first end E201 and the second end E202 are partially butted against each other at an angle. In the region where the first end E201 and the second end E202 are partially butted against each other at an angle, the intermediate layer 212 of the first end E201 is welded to the outermost layer 211 of the second end E202. In the region where the first end E201 and the second end E202 are partially butted against each other at an angle, the intermediate layer 212 of the second end E202 is welded to the innermost layer 213 of the first end E201.
[0114] The outermost layer 211 is made of paper. The thickness of the outermost layer 211 is 180 μm. The intermediate layer 212 has a two-layer structure. That is, the intermediate layer 212 includes a first layer and a second layer. The first layer and the second layer are stacked in this order from the outside in. The first layer is made of polyethylene (PE). The thickness of the first layer is 30 μm. The second layer is made of polyethylene terephthalate (PET). The thickness of the second layer is 12 μm. The innermost layer 213 is made of polyethylene (PE). The thickness of the innermost layer 213 is 150 μm.
[0115] The surface of the outermost layer 211 may be made of paper only. In this case, since there is no plastic coating the surface of the paper, it is possible to reduce the amount of plastic used in the tube container 300 and the proportion of plastic in the tube container 300. Greaseproof paper or waterproof paper can be used as the paper for the outermost layer 211. The surface of the paper for the outermost layer 211 may be varnished or ink-coated.
[0116] The configuration of the tape material 220 of this embodiment will be described in detail. The tape material 220 includes an inner layer 221 and an outer layer 222. The inner layer 221 covers the outer surface of the sheet material 210. The inner layer 221 is made of a thermoplastic resin. The inner layer 221 is impregnated into the paper of the outermost layer 211 of the sheet material 210. The outer layer 222 is overlaid on the inner layer 221. The inner layer 221 and the outer layer 222 are laminated in this order from the inside out. The thickness of the inner layer 221 is 80 μm. The thickness of the outer layer 222 is 12 μm. The inner layer 221 has a lower melting point than the outer layer 222.
[0117] The thermal conductivity of the outer layer 222 is lower than that of the inner layer 221. The inner layer 221 has a melting point that is 20°C or more lower than that of the outer layer 222. The inner layer 221 is made of polyethylene (PE), and the outer layer 222 is made of polyethylene terephthalate (PET). The melting point of polyethylene (PE) is lower than that of polyethylene terephthalate (PET). The inner layer 221 may be made of polyethylene (PE), and the outer layer 222 may be made of biaxially oriented polypropylene (PP). The melting point of polyethylene (PE) is lower than that of biaxially oriented polypropylene (PP). The inner layer 221 includes a barrier layer. The barrier layer has barrier properties.
[0118] Polyethylene (PE) has a higher thermal conductivity and a lower melting point than polypropylene (PP) and polyethylene terephthalate (PET). In addition, materials with a high melting point would affect the body of the tube container 300, so polyethylene (PE) is preferable.
[0119] When the tube container 300 is repeatedly bent, interfacial peeling may occur at the end of the tape material 220. When the depth to which the thermoplastic resin of the tape material 220 has impregnated the outermost layer 211 of the sheet material 210 is 5 μm or less, interfacial peeling is likely to occur. When the depth to which the thermoplastic resin of the tape material 220 has impregnated the outermost layer 211 of the sheet material 210 is more than 5 μm and less than 10 μm, interfacial peeling is unlikely to occur. When the depth to which the thermoplastic resin of the tape material 220 has impregnated the outermost layer 211 of the sheet material 210 is more than 10 μm and less than 15 μm, interfacial peeling is suppressed. When the depth to which the thermoplastic resin of the tape material 220 has impregnated the outermost layer 211 of the sheet material 210 is more than 15 μm, interfacial peeling is further suppressed.
[0120] Another example of the configuration of the tape material 220 will be described. When the adhesive surface of the substrate is polyethylene (PE), the tape material 220 is laminated in the following order from the inside: low-density polyethylene (LDPE), polyethylene terephthalate (PET), and low-density polyethylene (LDPE). When the adhesive surface of the substrate is solid polypropylene (CPP), the tape material 220 is laminated in the following order from the inside: solid polypropylene (CPP), oriented polypropylene (OPP), and solid polypropylene (CPP). When the adhesive surface of the substrate is heat-sealed polyethylene terephthalate (PET), the tape material 220 is laminated in the following order from the inside: heat-sealed polyethylene terephthalate (PET), oriented polyethylene terephthalate (PET), and heat-sealed polyethylene terephthalate (PET).
[0121] Furthermore, in the case of a substrate such as paper or cloth that is impregnated with the resin of the molten tape, the tape material 220 is layered in the order of low density polyethylene (LDPE), polyethylene terephthalate (PET), and low density polyethylene (LDPE) from the inside out.
[0122] In another example of the tape material 220 described above, the tape material 220 has the same structure on both sides, but the tape material 220 may not have the outer layer 222. For example, the tape material 220 may be made of low density polyethylene (LDPE) or polyethylene terephthalate (PET) from the inside.
[0123] However, it is desirable that the difference in melting point between the combined materials be 10° C. or more, and more desirably 20° C. or more. Furthermore, it is desirable that the tape material 220 has as little elongation as possible. Therefore, among base materials with high melting points, polyethylene terephthalate (PET), unstretched polypropylene (CPP), polytrimethylene terephthalate (PEN), polybutylene terephthalate (PBT), etc. have excellent processability.
[0124] The depth to which the thermoplastic resin of the tape material 220 has impregnated the outermost layer 211 of the sheet material 210 is 3 μm or more and 20 μm or less. The impregnation depth is about 10 μm when the heat, time, and resin selection are high temperature, long time, and high fluidity, respectively. The impregnation depth also depends on the surface condition of the paper, being about 3 μm for dense paper (coated paper, etc.) and about 20 μm for sparse paper (uncoated paper, etc.).
[0125] The tape material 220 may be a single layer. The single layer of the tape material 220 may be made of polyethylene (PE). Alternatively, the tape material 220 may have a three-layer structure. The three layers of the tape material 220 may be laminated in the following order from the inside out: polyethylene (PE), polyethylene terephthalate (PET), and polyethylene (PE). In this case, considering the possibility of a decrease in the adhesive strength of the adhesive layer and the possibility of exposure of the edge of the tape material 220, the tape material 220 may have the same structure on both sides, thereby protecting the edge of the tape material 220. Furthermore, by having the same structure on both sides of the tape material 220, it is possible to prevent confusion between the front and back of the tape material 220. By combining a sealant layer with a material with high rigidity, melting point (softening point), bending moment (MI), thermal conductivity, etc., meandering, cutting, stretching, etc. of the tape material 220 are suppressed. This increases the productivity of the tape material 220.
[0126] Next, modified examples of the tube container 300 according to this embodiment will be described. The configuration of a first modified example of the tube container 300 according to this embodiment will be described with reference to Fig. 16. Fig. 16 is an end view showing a portion corresponding to Fig. 15.
[0127] In a first modified example of the tube container 300 according to the present embodiment, the sheet material 210 includes a first end E201 and a second end E202 that are butted against each other. At the boundary where the first end E201 and the second end E202 are butted against each other, the outermost layer 211, the middle layer 212, and the innermost layer 213 of each of the first end E201 and the second end E202 are butted against each other. The tape material 220 covers from the outermost layer of the sheet material 210 to the first end E201 and the second end E202. The tape material 220 covers the boundary where the first end E201 and the second end E202 are butted against each other.
[0128] The configuration of a second modified example of the tube container 300 according to this embodiment will be described with reference to Fig. 17. Fig. 17 is an end view showing a portion corresponding to Fig. 15.
[0129] In a second modified example of the tube container 300 according to the present embodiment, the sheet material 210 includes a first end E201 and a second end E202 that are butted against each other. At the boundary where the first end E201 and the second end E202 are butted against each other, the innermost layers 213 of the first end E201 and the second end E202 are welded to each other. The innermost layers 213 of the first end E201 and the second end E202 are disposed between the outermost layers 211 and the middle layer 212 of the first end E201 and the second end E202. The innermost layers 213 of the first end E201 and the second end E202 form part of the outer surface of the sheet material 210. The tape material 220 covers the outermost layers of the sheet material 210, as well as the first end E201 and the second end E202. The tape material 220 covers the boundary where the first end E201 and the second end E202 are butted against each other. The tape material 220 covers the outermost layer 211, the middle layer 212, and the innermost layer 213 of each of the first end E201 and the second end E202.
[0130] Next, the effects of the tube container 300 according to this embodiment will be described. According to the tube container 300 according to this embodiment, the sheet material 210 includes paper in the outermost layer 211. This allows the appearance of the tube container 300 to have a paper-like texture. Furthermore, the thermoplastic resin of the tape material 220 is impregnated into the paper of the outermost layer 211 of the sheet material 210. This allows the thermoplastic resin of the tape material 220 to impregnate the paper of the outermost layer 211 of the sheet material 210, thereby achieving an anchoring effect. This allows the tape material 220 to improve the bonding strength between the first end E201 and the second end E202 of the sheet material 210. Therefore, sufficient bonding strength can be achieved even when paper is used in the outermost layer 211.
[0131] Furthermore, the sheet material 210 includes paper in the outermost layer 211. This allows for a reduction in the amount of plastic used in the tube container 300. Furthermore, the proportion of plastic in the tube container 300 can be reduced.
[0132] According to the tube container 300 of this embodiment, the inner layer 221 has a lower melting point than the outer layer 222. Therefore, when the first end E201 and the second end E202 of the sheet material 210 are joined by heat welding, the heat welding is performed at a temperature higher than the melting point of the inner layer 221 and lower than the melting point of the outer layer 222, thereby melting the inner layer 221 without melting the outer layer 222. Therefore, sufficient joining strength can be achieved by melting the thermoplastic resin of the inner layer 221 of the tape material 220 while not melting the outer layer 222.
[0133] According to the tube container 300 of this embodiment, the thermal conductivity of the outer layer 222 is lower than the thermal conductivity of the inner layer 221. Therefore, when the first end E201 and the second end E202 of the sheet material 210 are joined by thermal welding, heat is transferred more to the inner layer 221 than to the outer layer 222, thereby melting the thermoplastic resin of the inner layer 221 while preventing the outer layer 222 from melting. Therefore, sufficient joining strength can be achieved by melting the thermoplastic resin of the inner layer 221 of the tape material 220 while preventing the outer layer 222 from melting.
[0134] According to the tube container 300 of this embodiment, the inner layer 221 has a melting point that is 20° C. or more lower than that of the outer layer 222. Therefore, when the first end E201 and the second end E202 of the sheet material 210 are joined by heat welding, the heat welding is performed at a temperature that is higher than the melting point of the inner layer 221 and lower than the melting point of the outer layer 222 by 20° C. or more. This makes it possible to melt the inner layer 221 while preventing the outer layer 222 from melting. This makes it easy to melt the thermoplastic resin of the inner layer 221 of the tape material 220 while preventing the outer layer 222 from melting.
[0135] In the tube container 300 according to this embodiment, the inner layer 221 is made of polyethylene (PE), and the outer layer 222 is made of polyethylene terephthalate (PET). The melting point of polyethylene (PE) is lower than that of polyethylene terephthalate (PET). Therefore, when joining the first end E201 and the second end E202 of the sheet material 210 by thermal welding, sufficient joining strength can be achieved by melting the polyethylene (PE) of the inner layer 221 while preventing the polyethylene terephthalate (PET) of the outer layer 222 from melting.
[0136] In the tube container 300 according to this embodiment, the inner layer 221 is made of polyethylene (PE), and the outer layer 222 is made of biaxially oriented polypropylene (PP). The melting point of polyethylene (PE) is lower than that of biaxially oriented polypropylene (PP). Therefore, when joining the first end E201 and the second end E202 of the sheet material 210 by thermal welding, sufficient joining strength can be achieved by melting the polyethylene (PE) of the inner layer 221 while not melting the biaxially oriented polypropylene (PP) of the outer layer 222.
[0137] According to the tube container 300 of this embodiment, the inner layer 221 includes a barrier layer, which can improve the barrier properties at the boundary between the first end E201 and the second end E202 of the sheet material 210.
[0138] According to the tube container 300 of this embodiment, the depth to which the thermoplastic resin of the tape material 220 has impregnated the outermost layer 211 of the sheet material 210 is 3 μm or more and 20 μm or less. Therefore, the anchor effect caused by the thermoplastic resin of the tape material 220 impregnating the paper of the outermost layer 211 of the sheet material 210 can be ensured.
[0139] Examples of the present invention will be described below in comparison with comparative examples. Unless otherwise specified, the examples of the present invention have the same configuration as the tube container of the present embodiment.
[0140] In the tube container of Example 1, the thermoplastic resin of the tape material impregnated the outermost layer of the sheet material to a depth of 3 μm. The outermost paper layer of the sheet material was uncoated paper. The tape material was layered in the following order from the inside: low-density polyethylene (LDPE) with a thickness of 20 μm, polyethylene terephthalate (PET) with a thickness of 12 μm, and low-density polyethylene (LDPE) with a thickness of 20 μm.
[0141] In the tube container of Example 2, the thermoplastic resin of the tape material was impregnated into the outermost layer of the sheet material to a depth of 10 μm. The outermost paper layer of the sheet material was uncoated paper. The tape material was layered in the following order from the inside: 40 μm thick low-density polyethylene (LDPE), 12 μm thick polyethylene terephthalate (PET), and 40 μm thick low-density polyethylene (LDPE).
[0142] In the tube container of Example 3, the thermoplastic resin of the tape material impregnated the outermost layer of the sheet material to a depth of 15 μm. The outermost paper layer of the sheet material was uncoated paper. The tape material was layered in the following order from the inside: low-density polyethylene (LDPE) with a thickness of 60 μm, polyethylene terephthalate (PET) with a thickness of 12 μm, and low-density polyethylene (LDPE) with a thickness of 60 μm.
[0143] In the tube container of Example 4, the thermoplastic resin of the tape material was impregnated into the outermost layer of the sheet material to a depth of 5 μm. The outermost paper layer of the sheet material was uncoated paper. The tape material was layered in the following order from the inside: 30 μm thick low-density polyethylene (LDPE), 30 μm thick high-density polyethylene (HDPE), and 30 μm thick low-density polyethylene (LDPE).
[0144] In the tube container of Comparative Example 1, the thermoplastic resin of the tape material was impregnated into the outermost layer of the sheet material to a depth of 1 μm. The outermost layer of the sheet material was coated paper. The tape material was layered in the following order from the inside: low-density polyethylene (LDPE) with a thickness of 20 μm, polyethylene terephthalate (PET) with a thickness of 12 μm, and low-density polyethylene (LDPE) with a thickness of 20 μm.
[0145] In the tube container of Comparative Example 2, the thermoplastic resin of the tape material impregnated the outermost layer of the sheet material to a depth of 25 μm. The outermost paper layer of the sheet material was uncoated paper. The tape material was layered in the following order from the inside: 100 μm thick low-density polyethylene (LDPE), 12 μm thick polyethylene terephthalate (PET), and 100 μm thick low-density polyethylene (LDPE).
[0146] The bonding strength was insufficient in Comparative Example 1. In Comparative Example 2, the melted tape material protruded outside the heater when bonding by thermal welding, which impaired the aesthetic appearance.
[0147] In Examples 1 to 4, sufficient bonding strength was achieved. Furthermore, in Examples 1 to 4, the melted tape material did not protrude beyond the heater during thermal welding, thereby preventing aesthetic degradation. (Embodiment 4) The configuration of a tube container 400 according to Embodiment 4 will be described with reference to FIGS. 13 and 18 . The tube container 400 includes a sheet material 310 and a tape material 320. The sheet material 310 has a first end E301 and a second end E302 that partially overlap and partially butt together at an angle. Specifically, the first end E301 covers the second end E302 from the outside. The first end E301 is one end in the width direction of the sheet material 310, and the second end E302 is the other end in the width direction of the sheet material 310. The first end E301 is a first end that is a region having a width extending toward the second end E302. The second end E302 is a second end portion that is a region having a width toward the first end E301 side.
[0148] The tape material 320 covers the first end E301 and the second end E302 of the sheet material 310. The tape material 320 covers a portion of the inner surface of the sheet material 310. The tape material 320 may cover the first end E301 and the second end E302 continuously from the leading end to the trailing end of the sheet material 310 in the length direction perpendicular to the width direction of the sheet material 310.
[0149] 18 and 19 , the sheet material 310 includes an intermediate layer 311, an inner layer 312, and an outer layer 313. The intermediate layer 311 is sandwiched between the inner layer 312 and the outer layer 313. The inner layer 312 is disposed inside the intermediate layer 311. The outer layer 313 is disposed outside the intermediate layer 311. The intermediate layer 311, the inner layer 312, and the outer layer 313 are laminated in this order from the outside in the order of outer layer 313, intermediate layer 311, and inner layer 312. The intermediate layer 311 includes paper. The inner layer 312 and the outer layer 313 are made of a thermoplastic resin.
[0150] The tape material 320 is welded to at least one of the inner layer 312 and the outer layer 313 of the sheet material 310. In this embodiment, the tape material 320 is welded to the inner layer 312 of the sheet material 310. The tape material 320 is not welded to the outer layer 313 of the sheet material 310.
[0151] The structure of the sheet material 310 of this embodiment will be described in detail. In the region where the first end E301 and the second end E302 partially overlap each other, the outer layer 313 of the first end E301 overlaps the outer surface of the outer layer 313 of the second end E302. In the region where the first end E301 and the second end E302 partially overlap each other, the inner layer 312 of the second end E302 overlaps the inner surface of the inner layer 312 of the first end E301.
[0152] Between the overlapping regions of the first end E301 and the second end E302, there is provided a region where the first end E301 and the second end E302 are partially butted against each other at an angle. The intermediate layer 311 of the first end E301 is welded to the outer layer 313 of the second end E302. In the region where the first end E301 and the second end E302 are partially butted against each other at an angle, the intermediate layer 311 of the first end E301 is welded to the outer layer 313 of the second end E302. The intermediate layer 311 of the second end E302 is welded to the inner layer 312 of the first end E301. In the region where the first end E301 and the second end E302 are partially butted against each other at an angle, the intermediate layer 311 of the second end E302 is welded to the inner layer 312 of the first end E301.
[0153] The angle A between the first end E301 and the second end E302 of the sheet material 310, which are partially butted together at an angle, is 15° or more and 75° or less. The angle A is the angle formed by the boundary surface of the first end E301 and the second end E302, which are partially butted together at an angle, with respect to the extending direction perpendicular to the stacking direction in which the intermediate layer 311, the inner layer 312, and the outer layer 313 are stacked. The angle A is preferably 45° or more.
[0154] The dimension L in the thickness direction of the sheet material 310 at the first end E301 and the second end E302 that are partially overlapped with each other is greater than 0 mm and equal to or less than 0.5 mm.
[0155] The outer layer 313 is made of polyethylene (PE) and has a thickness of 150 μm. The inner layer 312 is made of polyethylene (PE) and has a thickness of 150 μm.
[0156] Another example of the structure of sheet material 310 of this embodiment will be described. Outer layer 313 may be made of polyethylene (PE) and have a thickness of 80 μm, and intermediate layer 311 may have a two-layer structure, in which, from the outer layer 313 side, the first layer may be made of paper and have a thickness of 180 μm, the second layer may be made of polyethylene terephthalate (PET) and have a thickness of 12 μm, and inner layer 312 may be made of polyethylene (PE) and have a thickness of 40 μm.
[0157] The outer layer 313 may be made of polyethylene (PE) and have a thickness of 20 μm, and the intermediate layer 311 may have a six-layer structure, in which, from the outer layer 313 side, the first layer may be made of paper and have a thickness of 70 μm, the second layer may be made of polyethylene (PE) and have a thickness of 15 μm, the third layer may be made of paper and have a thickness of 120 μm, the fourth layer may be made of ethylene-methacrylic acid copolymer (EMAA) and have a thickness of 20 μm, the fifth layer may be made of linear low-density polyethylene (LLDPE) and have a thickness of 80 μm, and the sixth layer may be made of vacuum-deposited polyethylene terephthalate (VMPET) and have a thickness of 12 μm, and the inner layer 312 may be made of polyethylene (PE) and have a thickness of 120 μm.
[0158] The outer layer 313 is made of ethylene-vinyl acetate copolymer (EVA), and the intermediate layer 311 has a four-layer structure, in which, from the outer layer 313 side, the first layer is paper and has a thickness of 200 μm, the second layer is ethylene-methacrylic acid copolymer (EMAA) and has a thickness of 20 μm, the third layer is aluminum (AL) and has a thickness of 9 μm, the fourth layer is polyethylene terephthalate (PET) and has a thickness of 12 μm, and the inner layer 312 may be polyethylene (PE) and has a thickness of 120 μm.
[0159] The outer layer 313 may be made of polyethylene (PE) and have a thickness of 15 μm, and the intermediate layer 311 may have a three-layer structure, in which, from the outer layer 313 side, the first layer is paper and has a thickness of 150 μm, the second layer is ethylene-methacrylic acid copolymer (EMAA) and has a thickness of 20 μm, the third layer is vacuum-deposited polyethylene terephthalate (VMPET) and has a thickness of 12 μm, and the inner layer 312 may be polyethylene (PE) and has a thickness of 80 μm.
[0160] The outer layer 313 may be made of polyethylene (PE) and have a thickness of 30 μm, and the intermediate layer 311 may have a three-layer structure, in which, from the outer layer 313 side, the first layer is paper and has a thickness of 120 μm, the second layer is ethylene-methacrylic acid copolymer (EMAA) and has a thickness of 20 μm, the third layer is vacuum-deposited polyethylene terephthalate (VMPET) and has a thickness of 12 μm, and the inner layer 312 may be polyethylene (PE) and have a thickness of 120 μm.
[0161] The outer layer 313 may be made of polyethylene (PE) and have a thickness of 20 μm, and the intermediate layer 311 may have a four-layer structure, in which, from the outer layer 313 side, the first layer may be made of paper and have a thickness of 180 μm, the second layer may be made of ethylene-methacrylic acid copolymer (EMAA) and have a thickness of 20 μm, the third layer may be made of aluminum (AL) and have a thickness of 9 μm, and the fourth layer may be made of ethylene-methacrylic acid copolymer (EMAA) and have a thickness of 30 μm, and the inner layer 312 may be made of polyethylene (PE) and have a thickness of 80 μm.
[0162] The outer layer 313 is made of polyethylene (PE) and has a thickness of 30 μm, and the intermediate layer 311 has a two-layer structure, in which, from the outer layer 313 side, the first layer is paper and has a thickness of 250 μm, and the second layer is polyethylene (PE) and has a thickness of 20 μm, and the inner layer 312 may be a co-extruded film of polyethylene (PE), ethylene-vinyl alcohol copolymer (EVOH), and polyethylene (PE) and has a thickness of 120 μm.
[0163] The outer layer 313 may be made of polyethylene (PE) and have a thickness of 30 μm, and the intermediate layer 311 may have a four-layer structure, in which, from the outer layer 313 side, the first layer may be made of paper and have a thickness of 100 μm, the second layer may be made of ethylene-methacrylic acid copolymer (EMAA) and have a thickness of 20 μm, the third layer may be made of aluminum (AL) and have a thickness of 9 μm, and the fourth layer may be made of polyethylene terephthalate (PET) and have a thickness of 12 μm, and the inner layer 312 may be made of polyethylene (PE) and have a thickness of 120 μm.
[0164] The configuration of the tape material 320 of this embodiment will be described in detail. The tape material 320 includes a first layer 321 and a second layer 322. The tape material 320 is laminated in the order of the first layer 321 and the second layer 322 from the inside out. The material of the first layer 321 is polyethylene (PE). The thickness of the first layer 321 is 80 μm. The material of the second layer 322 is polyethylene terephthalate (PET). The thickness of the second layer 322 is 12 μm.
[0165] Another example of the configuration of the tape material 320 of this embodiment will be described. The first layer 321 may be made of polyethylene (PE) and have a thickness of 30 μm, and the second layer 322 may be made of polyethylene terephthalate (PET) and have a thickness of 12 μm.
[0166] The tape material 320 may have a three-layer structure. The three layers of the tape material 320 may be laminated in the following order from the inside: polyethylene (PE), polyethylene terephthalate (PET), and polyethylene (PE). The thickness of the polyethylene (PE) may be 30 μm, and the thickness of the polyethylene terephthalate (PET) may be 25 μm.
[0167] The thickness of the polyethylene (PE) may be 20 μm, and the thickness of the polyethylene terephthalate (PET) may be 12 μm.
[0168] The tape material 320 may be a single layer. The single layer of the tape material 320 may be made of polyethylene (PE).
[0169] The width of the tape material 320 is 4 mm or more and 15 mm or less. From the viewpoint of reinforcement, the width of the tape material 320 is desirably 4 mm or more. The width of the tape material 320 is desirably 15 mm or less so that it is narrower than the width of the heater for welding.
[0170] Next, a modified example of the tube container 400 according to this embodiment will be described with reference to Fig. 20. Fig. 20 is an end view showing a portion corresponding to Fig. 19 .
[0171] In a modified example of the tube container 400 according to the present embodiment, the tape material 320 is welded to both the inner layer 312 and the outer layer 313 of the sheet material 310. The tape material 320 is arranged so as to be offset from each other in the inner layer 312 and the outer layer 313. The tape material 320 includes a first member 320a and a second member 320b. The first member 320a and the second member 320b have the same configuration. The first member 320a is arranged on the inner surface of the sheet material 310. The second member 320b is arranged on the outer surface of the sheet material 310. The first member 320a and the second member 320b are arranged so as to be offset from each other in the extending direction of the sheet material 310.
[0172] It is desirable that the width of the first member 320 a arranged on the inner surface of the sheet material 310 be equal to or greater than the width of the second member 320 b arranged on the outer surface of the sheet material 310 .
[0173] The width of the first member 320a disposed on the inner surface of the sheet material 310 may be 2.5 mm before processing. The first member 320a is fully melted on the heater to ensure a complete seal. When pressed by a heater with a width of 8 mm to 10 mm, the first member 320a is melted, compressed, and expanded, narrowing the width of the first member 320a. The reason for raising the melting temperature of the inner side of the sheet material 310 higher than the melting temperature of the outer side is that the inner side comes into contact with the contents, so the sealant must completely cover the contents, and the cross section of the tape material 320 must also be covered.
[0174] The width of the second member 320b arranged on the outer surface of the sheet material 310 may be 4 mm before processing. To avoid damaging the appearance, the outer side is melted at a lower temperature than the inner side. However, since it is necessary to connect the left and right end faces of the base material, the outer side is wider for strength reasons.
[0175] Next, the effects of the tube container 400 according to this embodiment will be described. According to the tube container 400 according to this embodiment, the intermediate layer 311 contains paper. This allows for a reduction in the amount of plastic used in the tube container 400. Furthermore, by welding the tape material 320 so as to cover the first end E301 and the second end E302 of the sheet material 310, which are partially overlapped and partially butted together at an angle, the welding strength at the first end E301 and the second end E302 can be improved.
[0176] Furthermore, the first end E301 and the second end E302 of the sheet material 310 are partially overlapped and partially butted together at an angle. This allows the weld length (length of the weld line) to be longer than when the first end E301 and the second end E302 are butted together perpendicularly. This improves the weld strength at the first end E301 and the second end E302.
[0177] According to the tube container 400 of this embodiment, the intermediate layer 311 of the first end E301 is welded to the outer layer 313 of the second end E302, and the intermediate layer 311 of the second end E302 is welded to the inner layer of the first end E301. Therefore, the outer layer 313 of the first end E301 overlaps the outer layer 313 of the second end E302, and the inner layer 312 of the second end E302 overlaps the inner layer 312 of the first end E301. Therefore, overlapping the outer and inner sides of the sheet material 310 can improve welding strength.
[0178] In the tube container 400 according to the present embodiment, the angle A between the first end E301 and the second end E302 of the sheet material 310, which are partially butted together at an angle, is 15° or more and 75° or less. This makes it possible to ensure ease of cutting the thin sheet material 310 while ensuring the welding length.
[0179] In the tube container 400 according to the present embodiment, the dimension L in the thickness direction of the sheet material 310 at the first end E301 and the second end E302 that partially overlap each other is greater than 0 mm and equal to or less than 0.5 mm. Therefore, the amount of overlap can be ensured while ensuring the sealing performance of the tape material 320.
[0180] According to the tube container 400 of this embodiment, the width of the tape material 320 is 4 mm or more and 15 mm or less. The melting point of polyethylene is lower than the melting point of polyethylene terephthalate. Therefore, by making the width of the tape material 320 narrower than the width of the welding heater while ensuring reinforcement by the tape material 320, welding strength can be ensured.
[0181] According to the tube container 400 of this embodiment, the tape material 320 is welded to both the inner layer 312 and the outer layer 313 of the sheet material 310. The tape material 320 is arranged so that it is offset from the inner layer 312 and the outer layer 313. As a result, the thickness does not become thick only at the attached portion of the tape material 320, but the thickness changes gradually, resulting in excellent end sealing properties. In addition, since there is little variation in the thickness of the sheet material 310, after-printing properties are high. Furthermore, since there is little unevenness in the sealed portion, the appearance is good. (Examples Related to Embodiment 1) Below, Examples A and B related to Embodiment 1 will be described.
[0182] Table 2 shows the structure and thickness of each layer of Example A, and Table 3 shows the structure and thickness of each layer of Example B. In the tables, the upper side of the table corresponds to the outside of the paper laminate tube, and the lower side of the table corresponds to the inside of the paper laminate tube. In addition, in Tables 2 and 3, the paper substrate has the same thickness.
[0183] In Table 2, PE1 and PE2 are polyethylene films, with PE1 corresponding to the second surface resin layer 23 in FIG. 6 and PE2 corresponding to the first surface resin layer 22 in FIG. 6. EXPE1 and EXPE2 are extruded polyethylene resins. EXPE1, although not shown in FIG. 6, is provided between the second surface resin layer 23 and the paper substrate 21. EXPE2 corresponds to the first adhesive layer 25 in FIG. 6. The paper substrate 150g corresponds to the single-layer paper 21a in FIG. 6. GLPET is a transparent vapor-deposited film and corresponds to the barrier layer 24 in FIG. 6. Although not shown in Table 2, there is another adhesive layer between GLPET and PE2. This adhesive layer is a two-component curing urethane adhesive, and it bonds GLPET and PE2 together by dry lamination. This adhesive layer corresponds to the second adhesive layer 26 in FIG. 6. The thickness of this adhesive layer is approximately 2 to 5 μm. The total thickness is the sum of each component and includes the thickness of any additional adhesive layers.
[0184]
[0185] Table 3 differs from Table 2 in that EXPE2 on the underside of the paper substrate (inside the paper laminate tube) is omitted and some of the thicknesses of each component are different. Furthermore, the aforementioned separate adhesive layer is provided not only between GLPET and PE2 but also between the paper substrate and GLPET. The paper substrate and GLPET are bonded together by dry lamination using a separate adhesive layer, a two-component curing urethane adhesive.
[0186]
[0187] In both Tables 2 and 3, it was possible to suppress the cohesion and peeling of the paper (paper base material) that constitutes the body. In addition, in the configuration in Table 3, by omitting EXPE2 on the lower side of the paper (corresponding to the inside of the container) and further reducing the thickness of PE1 and PE2, it was possible to increase the paper conversion rate compared to the configuration in Table 2.
[0188] In Example B (Table 3), when the paper laminated tube had a diameter of Φ50 mm, a body height of 180 mm, and a spout weight of 2.7 g, the paper conversion rate was 50.1%.
[0189] Although the embodiments of the present disclosure have been described above, the above-described embodiments can be modified in various ways. Furthermore, the scope of the present invention is not limited to the above-described embodiments. The scope of the present invention is defined by the claims, and is intended to include all modifications within the meaning and scope of the claims.
[0190] Various aspects of the present disclosure are summarized below as appendices. (Appendix A1) A paper laminate tube comprising a body portion, the body portion being composed of a sheet member having a first side and a second side opposite the first side, the sheet member being bent into a cylindrical shape with the first side facing inward, the sheet member having a paper substrate, the paper substrate including a first single-layer paper. (Appendix A2) The paper laminate tube according to Appendix A1, wherein the first single-layer paper includes a plurality of first fibers and a plurality of second fibers, the length of each of the plurality of first fibers being longer than the length of each of the plurality of second fibers and being 4 mm or less, the length of each of the plurality of second fibers being 0.2 mm or more and 1.5 mm or less, and the first fiber content of the first single-layer paper being 50 percent or more. (Appendix A3) The paper laminate tube according to Appendix A1, wherein the basis weight of the first single-layer paper is less than 165 g / m2. (Appendix A4) The paper laminated tube according to Appendix A1, wherein the paper base further includes a second monolayer paper layered on the first monolayer paper. (Appendix A5) The paper laminated tube according to Appendix A4, wherein the paper base further includes a resin layer sandwiched between the first monolayer paper and the second monolayer paper, the resin layer impregnating the surface of the first monolayer paper and the surface of the second monolayer paper. (Appendix A6) The paper laminated tube according to Appendix A5, wherein the resin layer is made of a resin material having a melting point of 300°C or less. (Appendix A7) The paper laminated tube according to Appendix A5, wherein the distance between the center of the sheet member in the thickness direction and the resin layer is 10% or less of the thickness of the sheet member. (Appendix A8) A paper laminated tube as described in Appendix A1, wherein the sheet member, when not bent, has a first end and a second end which are both ends in a second direction perpendicular to a first direction corresponding to the longitudinal direction of the body portion, the sheet member, when bent into a cylindrical shape, has the first surface at the first end and the second surface at the second end adhered together, the sheet member has a first surface resin layer on the first surface and a second surface resin layer on the second surface, and the thickness of the first surface resin layer is equal to or greater than the thickness of the second surface resin layer.(Appendix A9) The paper laminated tube according to any one of Appendices A1 to A8, further comprising a spout having an opening communicating with the interior of the body, the spout being made of a resin material having an MFR of 0.5 g / 10 min or more, a maximum thickness of 2.0 mm or less, and welded to one end of the body in the longitudinal direction. (Appendix B1) A paper laminated tube comprising: a body; and a spout having an opening communicating with the interior of the body, the body being made of a sheet member having a first side and a second side opposite the first side, and bent into a cylindrical shape with the first side facing inward, the sheet member having a paper base material, and the spout being made of a resin material having an MFR of 0.5 g / 10 min or more, a maximum thickness of 2.0 mm or less, and welded to one end of the body in the longitudinal direction. (Appendix B2) The paper laminated tube according to Appendix B1, wherein the value obtained by dividing the weight of the paper base material by the weight of the paper laminated tube is 50 percent or more. (Appendix B3) A method for manufacturing a paper laminated tube, comprising the steps of: preparing a sheet member having a first surface and a surface opposite to the first surface, the sheet member having a paper base material; bending the sheet member into a cylindrical shape so that the first surface faces inward to form a body portion; forming a spout using a resin material by injection molding; and welding the spout to one end of the body portion in the longitudinal direction. (Appendix C1) A paper laminated tube comprising a body portion, the body portion being composed of a sheet member having a first side and a second side opposite the first side, and bent into a cylindrical shape with the first side facing inward, the sheet member having a paper base material, a film member, and a resin layer disposed between the paper base material and the film member, the paper base material being made of uncoated paper. (Appendix C2) The paper laminated tube according to Appendix C1, in which the resin layer is impregnated to a depth of 3 μm or more from the surface of the paper base material. (Appendix C3) The paper laminated tube according to Appendix C1, in which the whiteness of the uncoated paper is 70% or less.(Appendix C4) The paper laminated tube according to any one of Appendices C1 to C3, wherein the resin layer is made of a resin material having a melting point of 300°C or less. (Appendix C5) The paper laminated tube according to any one of Appendices C1 to C3, wherein the resin layer is made of a resin material having an MFR of 3 g / 10 min or more. (Appendix C6) The paper laminated tube according to any one of Appendices C1 to C3, wherein the surface of the paper base has a 10-point average roughness of 10 μm to 60 μm. (Appendix D1) A tube container comprising: a sheet material including paper in an outermost layer and including first and second ends that are overlapped or butted against each other; and a tape material covering the outermost layer of the sheet material, the first and second ends, the tape material including a thermoplastic resin, and the thermoplastic resin of the tape material impregnating the paper of the outermost layer of the sheet material. (Appendix D2) The tube container according to Appendix D1, wherein the tape material includes an inner layer made of the thermoplastic resin and impregnated into the paper of the outermost layer of the sheet material, and an outer layer superposed on the inner layer, the inner layer having a lower melting point than the outer layer. (Appendix D3) The tube container according to Appendix D2, wherein the thermal conductivity of the outer layer is lower than that of the inner layer. (Appendix D4) The tube container according to Appendix D2, wherein the inner layer has a melting point that is 20°C or more lower than that of the outer layer. (Appendix D5) The tube container according to Appendix D2, wherein the inner layer is made of polyethylene, and the outer layer is made of polyethylene terephthalate. (Appendix D6) The tube container according to Appendix D2, wherein the inner layer is made of polyethylene, and the outer layer is made of biaxially oriented polypropylene. (Appendix D7) The tube container according to Appendix D2, wherein the inner layer includes a barrier layer. (Appendix D8) The tube container according to Appendix D1, wherein the depth to which the thermoplastic resin of the tape material is impregnated into the outermost layer of the sheet material is 3 μm or more and 20 μm or less.(Appendix E1) A tube container comprising: a sheet material having first and second ends that are partially overlapping and partially butted together at an angle; and a tape material covering the first and second ends of the sheet material, wherein the sheet material includes an intermediate layer, an inner layer disposed inside the intermediate layer, and an outer layer disposed outside the intermediate layer, the intermediate layer including paper, and the inner and outer layers made of thermoplastic resin, and the tape material is welded to at least one of the inner and outer layers of the sheet material. (Appendix E2) The tube container according to Appendix E1, wherein the intermediate layer at the first end is welded to the outer layer at the second end, and the intermediate layer at the second end is welded to the inner layer at the first end. (Appendix E3) The tube container according to Appendix E1, wherein the angle between the first and second ends of the sheet material that are partially butted together at an angle is between 15° and 75°. (Appendix E4) The tube container according to Appendix E1, wherein the dimension in the thickness direction of the sheet material of the first end and the second end, which are partially overlapped with each other, is more than 0 mm and 0.5 mm or less. (Appendix E5) The tube container according to Appendix E1, wherein the width of the tape material is 4 mm or more and 15 mm or less. (Appendix E6) The tube container according to Appendix E1, wherein the tape material is welded to both the inner layer and the outer layer of the sheet material and is arranged so that the inner layer and the outer layer are offset from each other. (Appendix F1) A paper laminate tube comprising a body portion, wherein the body portion is composed of a sheet member having a first surface and a second surface opposite to the first surface and bent into a cylindrical shape so that the first surface faces inward, wherein the sheet member has a paper base material, and the paper base material includes a first single-layer paper. (Appendix F2) A paper laminate tube comprising a body portion, the body portion being made of a sheet member having a first surface and a second surface opposite to the first surface, and bent into a cylindrical shape so that the first surface faces inward, the sheet member having a paper base material, a film member, and a resin layer disposed between the paper base material and the film member, and the paper base material being made of uncoated paper.(Appendix F3) The paper laminated tube according to Appendix F1 or Appendix F2, wherein the sheet member includes the paper base material in its outermost layer and includes a first end and a second end that are overlapped or abutted against each other, and further includes a tape material covering the outermost layer of the sheet member to the first end and the second end, the tape material including a thermoplastic resin, and the thermoplastic resin of the tape material is impregnated into the paper base material in the outermost layer of the sheet member. (Appendix F4) The paper laminated tube according to Appendix F1 or Appendix F2, further includes a spout provided with an opening that communicates with the interior of the body, the spout being made of a resin material having an MFR of 0.5 g / 10 min or more, having a maximum thickness of 2.0 mm or less, and welded to one longitudinal end of the body. (Appendix F5) The paper laminated tube according to Appendix F1 or Appendix F2, wherein the sheet member has first and second ends that are partially overlapped and partially butted against each other at an angle, and a tape material covering the first and second ends of the sheet member, the sheet member including a middle layer, an inner layer disposed inside the middle layer, and an outer layer disposed outside the middle layer, the middle layer including the paper base material, the inner layer and the outer layer being made of a thermoplastic resin, and the tape material being welded to at least one of the inner layer and the outer layer of the sheet member. (Appendix F6) The paper laminated tube according to Appendix F1, wherein the paper base material further includes a second single-layer paper overlaid on the first single-layer paper. (Appendix F7) A paper laminate tube according to Appendix F6, wherein the paper base material further has a resin layer sandwiched between the first monolayer paper and the second monolayer paper, and the resin layer is impregnated into the surface of the first monolayer paper and also into the surface of the second monolayer paper.
[0191] 10 Body portion, 10a Opening, 20 Sheet member, 20a, 120a First surface, 20b 120b Second surface, 20c First end, 20d Second end, 21 Paper base material, 21a, 21b Single layer paper, 21c Resin layer, 22 First surface resin layer, 23 Second surface resin layer, 24 Barrier layer, 25 First adhesive layer, 26 Second adhesive layer, 27, 28 Resin layer, 30 Spout, 31 Protrusion, 31a Opening, 40 Cap, 100 Paper laminate tube, 122, 123 Sealant layer, 124 Film member, 125 Resin layer, 201 Body portion, 202 Spout portion, 203 Cap, 210 Sheet material, 211 Outermost layer, 212 Middle layer, 213 Innermost layer, 220 Tape material, 221 inner layer, 222 outer layer, 300, 400 tube container, 310 sheet material, 311 intermediate layer, 312 inner layer, 313 outer layer, 320 tape material, 321 first layer, 322 second layer, A angle, DIS distance, DR1 first direction, DR2 second direction, E201, E301 first end, E202, E302 second end, L dimension, S1 body forming process, S2 spout forming process, S3 spout welding process, T, T1, T2 thickness.
Claims
1. A paper laminate tube comprising: a body portion, the body portion being composed of a sheet member having a first surface and a second surface opposite the first surface, the sheet member being bent into a cylindrical shape with the first surface facing inward, the sheet member having a paper base material, the paper base material including a first monolayer paper.
2. A paper laminate tube comprising a body portion, the body portion being composed of a sheet member having a first surface and a second surface opposite to the first surface, the sheet member being bent into a cylindrical shape with the first surface facing inward, the sheet member having a paper base material, a film member, and a resin layer disposed between the paper base material and the film member, the paper base material being made of uncoated paper.
3. A paper laminate tube as described in claim 1 or claim 2, wherein the sheet member includes the paper base material in its outermost layer and includes a first end and a second end that are overlapped or abutted against each other, and further includes a tape material covering the outermost layer of the sheet member to the first end and the second end, the tape material including a thermoplastic resin, and the thermoplastic resin of the tape material is impregnated into the paper base material of the outermost layer of the sheet member.
4. A paper laminate tube as described in claim 1 or claim 2, comprising a spout having an opening communicating with the inside of the body, the spout being made of a resin material having an MFR of 0.5 g / 10 min or more, a maximum thickness of 2.0 mm or less, and welded to one end of the body in the longitudinal direction.
5. A paper laminate tube as described in claim 1 or claim 2, wherein the sheet member has first and second ends which are partially overlapped and partially butted together at an angle, and a tape material covers the first and second ends of the sheet member, the sheet member includes an intermediate layer, an inner layer disposed inside the intermediate layer, and an outer layer disposed outside the intermediate layer, the intermediate layer includes the paper base material, the inner layer and the outer layer are made of a thermoplastic resin, and the tape material is welded to at least one of the inner layer and the outer layer of the sheet member.
6. The paper laminate tube of claim 1, wherein the paper substrate further comprises a second monolayer paper layered on the first monolayer paper.
7. A paper laminate tube as described in claim 6, wherein the paper base material further has a resin layer sandwiched between the first monolayer paper and the second monolayer paper, and the resin layer is impregnated into the surface of the first monolayer paper and also into the surface of the second monolayer paper.
Citation Information
Patent Citations
Packing material for liquid vessel made of paper
JP1984093631A
Head of tubular container
JP1999321900A
Tube container
JP2015096431A
Liquid discharge container and combination body
JP2018065601A
Laminate and tube container
JP2022056686A