Thermally conductive composition

The thermally conductive composition with silicone and specific filler materials addresses the hardness and shape conformity issues of high thermal conductivity sheets by reducing compressive loads and maintaining high thermal performance, ensuring safe and effective heat dissipation for IC chips.

WO2024204441A1PCT designated stage expired Publication Date: 2024-10-03BANDO CHEM IND LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012455
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Thermally conductive sheets with high thermal conductivity become hard when filled with increased amounts of conductive fillers, requiring higher compressive loads for attachment to IC chips, which can cause damage and fail to conform to varying chip shapes, leading to continuous load application and potential chip failure.

Method used

A sheet-shaped thermally conductive composition comprising a resin composition with silicone and thermally conductive fillers, such as carbon fibers, scale-like graphite powder, and spherical zinc oxide particles, that maintains high thermal conductivity while reducing compressive load and allowing for easy deformation to follow IC chip shapes, with an initial compressive load of 1.0 N/mm² or less and a ratio of 0.5 or less after 1 minute, and an apparent thermal conductivity of 22.8 W/mK or more when compressed by 20%.

Benefits of technology

The composition effectively reduces the load on IC chips during attachment and follows the shape of heat-generating components, preventing continuous high load application and ensuring efficient heat dissipation while maintaining thermal conductivity, thus protecting the chips and enhancing heat transfer performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012455_03102024_PF_FP_ABST
    Figure JP2024012455_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A sheet-like thermally conductive composition comprising a resin composition containing a silicone and a thermally conductive filler. When subjected to 50% compression deformation, the initial compression load value is 1.0 N / mm2 or less, and the ratio of the compression load value after one minute has elapsed to the initial compression load value is 0.5 or less. The apparent thermal conductivity when subjected to 20% compression deformation is 22.8 W / mK or more.
Need to check novelty before this filing date? Find Prior Art

Description

Thermally conductive composition

[0001] The present application claims priority to Japanese Application No. 2023-053524, filed March 29, 2023, and incorporates by reference the entire contents of said Japanese application.

[0002] A heat-generating component such as an IC chip is usually attached to a heat-dissipating component such as a heat sink via a thermal interface material (TIM). Heat generated in the heat-generating component is conducted to the heat-dissipating component via the thermal interface material.

[0003] As the thermally conductive material, for example, a thermally conductive sheet has been proposed in which spherical alumina and carbon fibers are blended as thermally conductive fillers in a resin matrix (see Patent Documents 1 and 2).

[0004] International Publication No. 2019 / 244890 Japanese Patent Application Laid-Open No. 2014-31501

[0005] Thermally conductive sheets are components that are required to have excellent thermal conductivity, and their thermal conductivity can be increased by increasing the amount of thermally conductive filler they contain. On the other hand, thermally conductive sheets tend to become harder as the content of thermally conductive filler increases. Thermally conductive sheets used on IC chips are attached to the IC chips while applying a predetermined compressive load. Furthermore, the harder the thermally conductive sheet, the greater the compressive load that must be applied when attaching it to the IC chip.

[0006] Therefore, when attaching a hard thermally conductive sheet with high thermal conductivity to an IC chip, a relatively large compressive load must be applied. On the other hand, a large compressive load places a large load on the IC chip. If the compressive load applied during attachment is maintained afterward, the IC chip will continue to be subjected to a large load. The application of a large continuous load to the IC chip can cause the IC chip to fail.

[0007] Furthermore, a thermally conductive sheet may be attached to simultaneously cover multiple heat-generating components such as IC chips. In this case, the shapes of the heat-generating components are usually not the same, so the thermally conductive sheet is required to be able to deform to accommodate the different shapes of the heat-generating components.

[0008] Under these circumstances, the inventors of the present invention have conducted extensive research and have completed a thermally conductive composition that has excellent thermal conductivity, easily conforms to the shape of heat-generating components such as IC chips, and reduces the load on the heat-generating components.

[0009] A thermally conductive composition according to one embodiment of the present invention is a sheet-shaped thermally conductive composition made of a resin composition containing silicone and a thermally conductive filler, and has an initial compressive load value of 1.0 N / mm when compressed and deformed by 50%. 2 the ratio of the compressive load value after 1 minute to the initial compressive load value is 0.5 or less; and the apparent thermal conductivity when compressed and deformed by 20% is 22.8 W / mK or more.

[0010] A thermally conductive composition according to one embodiment of the present invention has high thermal conductivity. The thermally conductive composition is easily deformed to conform to the shape of a heat-generating component such as an IC chip. When the thermally conductive composition is attached to a heat-generating component such as an IC chip, the load on the IC chip can be reduced.

[0011] FIG. 1 is a cross-sectional view schematically illustrating an IC chip to which a heat sink is attached via a sheet-like thermally conductive composition according to an embodiment of the present invention. FIG. 2A is a perspective view schematically illustrating an example of a sheet-like thermally conductive composition according to an embodiment of the present invention. FIG. 2B is a partially enlarged view of the cross section taken along line A-A in FIG. 2A. FIG. 3 is a schematic cross-sectional view of the tip of an extruder and a T-die used in producing the sheet-like thermally conductive composition according to this embodiment. FIGS. 4A to 4D are views illustrating another example of a method for producing a sheet-like thermally conductive composition according to an embodiment of the present invention. FIGS. 5A to 5C are views illustrating a method for evaluating trackability in Examples and Comparative Examples.

[0012] The outline of the embodiments of the present invention will be described below. (1) A sheet-shaped thermally conductive composition comprising a resin composition containing silicone and a thermally conductive filler, wherein the initial compressive load value when compressed by 50% is 1.0 N / mm 2 a ratio of the compressive load value after 1 minute to the initial compressive load value is 0.5 or less, and the apparent thermal conductivity when compressed and deformed by 20% is 22.8 W / mK or more.

[0013] This sheet-shaped thermally conductive composition has high thermal conductivity and can reduce the load on the heat-generating component after installation. It also easily conforms to the shape of the heat-generating component during installation. Furthermore, even if the heat-generating component deforms due to heat after installation, the sheet-shaped thermally conductive composition can also conform to the deformation.

[0014] (2) In the thermally conductive composition of (1) above, the compressive load value after one minute is 0.4 N / mm 2 In this case, it is possible to avoid a high load being continuously applied to the IC chip after attachment.

[0015] (3) In the thermally conductive composition of (1) or (2) above, the resin composition preferably contains polydimethylsiloxane as the silicone. (4) In any of the thermally conductive compositions of (1) to (3) above, the resin composition preferably contains, as the thermally conductive filler, an anisotropic thermally conductive filler and a non-anisotropic thermally conductive filler. (5) In any of the thermally conductive compositions of (1) to (4) above, the resin composition preferably contains, as the thermally conductive filler, a fibrous filler, a scaly filler, and a spherical filler.

[0016] These resin compositions are suitable as resin compositions for constituting thermally conductive sheets that have high thermal conductivity and can reduce the load on IC chips.

[0017] (6) In the thermally conductive compositions of (1) to (5) above, the resin composition preferably contains carbon fiber, flake graphite powder, and spherical zinc oxide particles as thermally conductive fillers. When zinc oxide particles are contained as the thermally conductive filler, the thermal conductivity of the sheet-shaped thermally conductive composition is more easily increased than when alumina particles are contained. When carbon fiber and flake graphite powder are used in combination as the thermally conductive filler, the thermal conductivity of the sheet-shaped thermally conductive composition is more easily increased while suppressing the initial load than when only one of carbon fiber and flake graphite powder is contained.

[0018] (7) In the thermally conductive composition of (6) above, the total content of the carbon fiber, the scaly graphite powder, and the spherical zinc oxide particles is preferably 50% by volume or more and 70% by volume or less. (8) In the thermally conductive composition of (6) or (7) above, the content of the carbon fiber is preferably 30% by volume or more and 45% by volume or less. In these cases, it is more suitable for ensuring good thermal conductivity while suppressing the compressive load value required for 50% compressive deformation.

[0019] Hereinafter, a sheet-shaped thermally conductive composition according to an embodiment of the present invention will be described in detail, but the embodiment of the present invention is not limited to the following embodiment.

[0020] In an embodiment of the present invention, the "sheet-shaped thermally conductive composition" includes both a block-shaped product obtained by molding by extrusion molding or the like, and cut products (including sliced ​​sheet-shaped products) obtained by appropriately cutting the block-shaped product. Here, an embodiment of the sheet-shaped thermally conductive composition will be described using a sliced ​​sheet-shaped product as an example.

[0021] The sheet-shaped thermally conductive composition according to this embodiment is a component disposed between an IC chip and a heat sink. The thermally conductive composition is a resin composition containing silicone and a thermally conductive filler. Here, silicone is a polymeric compound having a main skeleton formed by siloxane bonds. FIG. 1 is a cross-sectional view schematically illustrating an IC chip to which a heat sink is attached via a sheet-shaped thermally conductive composition according to an embodiment of the present invention. FIG. 2A is a perspective view schematically illustrating an example of a sheet-shaped thermally conductive composition according to an embodiment of the present invention. FIG. 2B is a partially enlarged view of the cross section taken along line A-A in FIG. 2A. Note that all of the drawings in this application are schematic diagrams and do not accurately reflect the actual dimensions of each component.

[0022] As shown in Fig. 1, a sheet-like thermally conductive composition 1 (hereinafter also referred to as thermally conductive sheet 1) is placed between an IC chip 11 and a heat sink 12. The thermally conductive sheet 1 is used with one surface in contact with the IC chip 11 and the other surface in contact with the heat sink 12. In this way, the heat sink 12 is attached to the IC chip 11 via the thermally conductive sheet 1. Therefore, heat generated by the IC chip 11 is dissipated by the heat sink 12 to the outside of a housing (not shown).

[0023] 1 shows a usage mode of the thermally conductive sheet 1 attached to the upper surface of one IC chip 11. On the other hand, the sheet-shaped thermally conductive composition (thermally conductive sheet) according to an embodiment of the present invention may be a thermally conductive sheet that is attached so as to simultaneously cover heat-generating components such as multiple IC chips.

[0024] When the thermal conductive sheet 1 is compressed and deformed by 50% in the thickness direction (the vertical direction in FIGS. 2A and 2B), the initial compressive load value is 1.0 N / mm 2The following is an explanation. When attaching the thermally conductive sheet 1 to the IC chip 11, a predetermined load is applied to press the thermally conductive sheet 1 onto the IC chip 11. If the flexibility of the thermally conductive sheet 1 is insufficient, the thermally conductive sheet 1 and the IC chip 11 may not adhere to each other, resulting in a gap at the interface between them. Furthermore, when a single thermally conductive sheet 1 is attached to cover multiple heat-generating components simultaneously, it may not be able to conform to the shapes of all the heat-generating components, resulting in a gap between the sheet and one of the heat-generating components.

[0025] On the other hand, if the load when attaching the thermally conductive sheet 1 is increased, the thermally conductive sheet 1 and the IC chip 11 are closely attached to each other, making it difficult for gaps to form, but in this case, there is a risk of the IC chip 11 being damaged. 2 In many cases, the thermally conductive sheet 1 described below can be properly attached to an IC chip or the like within the range of the allowable compressive load specified for each IC chip. 2 The thermally conductive sheet 1 described below can easily conform to the shape of each heat-generating component when attached to cover multiple heat-generating components at the same time.

[0026] The initial compressive load value is 0.7 N / mm 2 It is preferable that the initial compressive load value is 0.1 N / mm or less. This is more suitable for adhering the thermally conductive sheet to the IC chip without applying a load to the IC chip. In the thermally conductive sheet 1, the initial compressive load value is usually 0.1 N / mm 2 Above, 0.1N / mm 2 It may be smaller.

[0027] The thermally conductive sheet 1 has a ratio of the compressive load value after 1 minute of being compressed 50% in the thickness direction (hereinafter referred to as the compressive load value after 1 minute) to the initial compressive load value of 0.5 or less. In this case, the thermally conductive sheet 1 easily deforms according to the shape of the IC chip 11. Therefore, it can follow the shape of the IC chip 11 when attached to the IC chip 11. It is particularly suitable for attachment so as to simultaneously cover multiple heat-generating components. Furthermore, if the IC chip 11 deforms due to heat, the thermally conductive sheet 1 easily deforms to follow that deformation. Furthermore, it is possible to avoid continuous high load on the IC chip.

[0028] The compressive load value of the thermal conductive sheet 1 after 1 minute was 0.4 N / mm 2 In this case, after the thermally conductive sheet 1 is attached to the IC chip 11 with a predetermined load applied thereto, the load is sufficiently released. Therefore, it is possible to avoid a large load being continuously applied to the IC chip 11 for a long period of time.

[0029] The compressive load value after 1 minute was 0.2 N / mm 2 More preferably, it is 0.15 N / mm or less. 2 The lower limit of the compressive load value after 1 minute is not limited, and it may be any value that allows the thermally conductive composition to maintain its sheet shape.

[0030] The initial compression load value when the thermal conductive sheet 1 is compressed and deformed by 50% in the thickness direction is measured using a universal testing machine (e.g., Instron 5969 (manufactured by Instron)) as a measuring instrument. The thermal conductive sheet 1 is compressed in the thickness direction at a compression rate of 5 mm / min to a thickness of "thickness before measurement x 0.5", and the load value at that time is measured. Furthermore, based on the obtained measurement value, the unit area (mm 2 The compressive load value per unit area (mm ) is calculated. The compressive load value after 1 minute is measured by measuring the load value after leaving the specimen for 1 minute in the state where the initial compressive load value was measured (a state where the specimen is compressed and deformed by 50% in the thickness direction). Furthermore, the compressive load value per unit area (mm ) is calculated based on the measured values. 2 ) and calculate the compression load value per

[0031] The thermal conductive sheet 1 has an apparent thermal conductivity of 22.8 W / mK or more when compressed and deformed by 20% in the thickness direction. If the apparent thermal conductivity is less than 22.8 W / mK, the thermal conductivity is insufficient. The apparent thermal conductivity of the thermal conductive sheet 1 is preferably 26.6 W / mK or more.

[0032] The apparent thermal conductivity of the thermal conductive sheet 1 is calculated by the thermal resistance (Kcm) measured when the sheet is compressed to a thickness of "thickness before measurement x 0.8" (20% compression). 2 / W) and the thickness (cm) of the thermally conductive sheet at the time of measurement, according to the following calculation formula (1).

[0033] Apparent thermal conductivity (W / mK) = thickness of thermal conductive sheet at time of measurement (cm) ÷ thermal resistance value when compressed and deformed by 20% (Kcm 2 / W)×100...(1)

[0034] The thermal resistance value when the thermal conductive sheet 1 is compressed and deformed by 20% is measured using a thermal conductivity measuring device (for example, TIMtester 1400 (manufactured by AnalysisTech)) in a state where the thermal conductive sheet 1 is compressed and deformed by 20%.

[0035] The thickness of the thermally conductive sheet 1 is not particularly limited, but is, for example, 0.05 mm or more and 3.0 mm or less. In this case, the thermally conductive sheet 1 can be suitably used as a member that efficiently transfers heat between the IC chip 11 and the heat sink 12. The thickness of the thermally conductive sheet 1 is preferably 0.05 mm or more and 2.5 mm or less. This ensures superior heat dissipation performance while ensuring conformability to the shapes of the IC chip 11 and the heat sink 12. On the other hand, if the thickness of the thermally conductive sheet 1 is less than 0.05 mm, it may not be able to fully conform to the shapes of the IC chip 11 and the heat sink 12. Furthermore, if the thickness exceeds 2.5 mm, the thermal resistance of the sheet itself may result in poor heat dissipation performance.

[0036] The planar shape of the thermally conductive sheet 1 is, for example, rectangular. In this case, the vertical and horizontal dimensions of the thermally conductive sheet 1 may be determined taking into consideration the dimensions of the member to which the thermally conductive sheet 1 is attached, such as the IC chip 11, and for example, both the vertical and horizontal dimensions are independently 10 mm to 120 mm. The planar shape of the thermally conductive sheet 1 is not limited to rectangular, and may be a shape other than rectangular, such as circular or elliptical. In the case of a circular shape, the diameter is, for example, 10 mm to 120 mm. In the case of an elliptical shape, the major axis or minor axis is, for example, 10 mm to 120 mm.

[0037] As shown in Figure 2B, the thermally conductive sheet 1 contains a matrix component 2 and a thermally conductive filler 4. In the thermally conductive sheet 1, all components other than the thermally conductive filler are collectively referred to as the matrix components. The thermally conductive sheet 1 may have weld lines formed in the thickness direction.

[0038] The matrix component 2 contains silicone. Therefore, the thermally conductive sheet 1 has excellent heat resistance. In this embodiment, the silicone may contain a cross-linked silicone (hereinafter also referred to as cross-linked silicone), but it is preferable that uncross-linked silicone is the main component from the viewpoint of easily ensuring good flexibility. Here, "mainly composed of uncross-linked silicone" means that the proportion of uncross-linked silicone in the entire silicone is 50 mass % or more. The silicone may be composed only of uncross-linked silicone. By using uncross-linked silicone as the main component, it becomes easier to release the load after attachment to an IC chip or the like.

[0039] The uncrosslinked silicone is preferably polydimethylsiloxane, which is a silicone whose side chains are all methyl groups and contain no unsaturated groups. The silicone preferably contains 50% by mass or more of the polydimethylsiloxane, more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more. The polydimethylsiloxane is a polymer with low reactivity and excellent stability. Therefore, by increasing the proportion of the polydimethylsiloxane in the silicone, the flexibility of the thermally conductive sheet 1 can be improved.

[0040] The polydimethylsiloxane may be an oil or a millable type, but millable type polydimethylsiloxane is preferred because it has good moldability when producing the thermally conductive sheet 1 by the method described below.

[0041] The molecular weight of the polydimethylsiloxane is preferably 60,000 or more and 700,000 or less in terms of mass average molecular weight MW. If the mass average molecular weight MW of the polydimethylsiloxane is less than 60,000, the polydimethylsiloxane tends to bleed out from the thermal conductive sheet 1. On the other hand, if the mass average molecular weight MW of the polydimethylsiloxane exceeds 700,000, the moldability and processability during production of the thermal conductive sheet 1 tend to be poor.

[0042] In the present invention, the weight average molecular weight MW of polydimethylsiloxane is a weight average molecular weight measured using gel permeation chromatography (GPC) using polystyrene as a standard substance in accordance with JIS-K7252-1:2008 "Plastics - Determination of average molecular weight and molecular weight distribution of polymers by size exclusion chromatography - Part 1: General rules."

[0043] The kinematic viscosity of the polydimethylsiloxane is preferably 10,000 cps or more and 100,000 cps or less, as measured with an Ubbelohde viscometer at 25° C. If the kinematic viscosity is less than 10,000 cps, the polydimethylsiloxane will tend to bleed out of the thermally conductive sheet 1. On the other hand, if the kinematic viscosity exceeds 100,000 cps, the hardness of the thermally conductive sheet 1 will increase, and when the thermally conductive sheet 1 is disposed between an IC chip and a heat sink, the sheet may have poor adhesion and conformability to the contact surfaces of the IC chip and the heat sink.

[0044] When the silicone contains a crosslinked silicone, the crosslinked silicone may be one that has been crosslinked by peroxide or one that has been crosslinked by an addition reaction, but one that has been crosslinked by peroxide is preferred. This is because crosslinked silicones that have been crosslinked by peroxide crosslinking have better heat resistance. Examples of the crosslinked silicone include those obtained by crosslinking silicones that have crosslinkable functional groups such as vinyl groups in part of their side chains (including terminals).

[0045] The silicone may contain silicone having a crosslinkable functional group such as a vinyl group in an uncrosslinked state.

[0046] The matrix component 2 may contain other elastomer components and the like to the extent that the required properties of the thermally conductive sheet 1 are not impaired.

[0047] The matrix component 2 may contain common additives such as flame retardants, reinforcing agents, fillers, softeners, plasticizers, antioxidants, tackifiers, antistatic agents, kneaded adhesives, and coupling agents. Examples of the flame retardants include magnesium hydroxide, aluminum hydroxide, platinum-based compounds, triazole-based compounds, iron oxides such as red iron oxide and black iron. These may be used alone or in combination of two or more. The magnesium hydroxide can also function as a thermally conductive filler.

[0048] The matrix component 2 preferably contains a coupling agent such as a silane coupling agent as an additive. In particular, when zinc oxide particles are contained as the thermally conductive filler, it is preferable to contain a silane coupling agent. By using a combination of zinc oxide particles and a silane coupling agent, the flexibility of the thermally conductive sheet 1 can be increased.

[0049] Examples of the silane coupling agent include methyltrimethoxysilane, ethyltrimethoxysilane, propyltrimethoxysilane, butyltrimethoxysilane, pentyltrimethoxysilane, hexyltrimethoxysilane, hexyltriethoxysilane, octyltrimethoxysilane, octyltriethoxysilane, decyltrimethoxysilane, decyltriethoxysilane, dodecyltrimethoxysilane, dodecyltriethoxysilane, hexadecyltrimethoxysilane, hexadecyltriethoxysilane, octadecyltrimethoxysilane, octadecyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, etc. These may be used alone or in combination of two or more.

[0050] The thermally conductive sheet 1 contains a thermally conductive filler 4. The thermally conductive filler 4 preferably contains an anisotropic thermally conductive filler (hereinafter also referred to as an anisotropic filler) and a non-anisotropic thermally conductive filler (hereinafter also referred to as a non-anisotropic filler). In this case, it is easy to ensure both high thermal conductivity and flexibility, and the moldability during manufacturing is also good. On the other hand, if the thermally conductive sheet 1 contains only an anisotropic filler, it is difficult to reduce the compression load value. Furthermore, cracks are likely to occur in the molded product during the manufacturing process. Furthermore, if the thermally conductive sheet 1 contains only a non-anisotropic filler, it is difficult to increase the thermal conductivity of the thermally conductive sheet 1.

[0051] In the thermally conductive filler, an anisotropic filler refers to a filler with an aspect ratio of 2.0 or more, and a non-anisotropic filler refers to a filler with an aspect ratio of less than 2.0. The aspect ratio of the thermally conductive filler refers to the larger of the ratio of the major axis of the filler to the minor axis of the filler and the ratio of the major axis of the filler to the thickness of the filler. The major axis, minor axis, and thickness correspond to the length, width, and height, respectively, of the circumscribed rectangular parallelepiped of the filler.

[0052] The anisotropic filler includes fibrous fillers, scaly fillers, plate-like fillers, flaky fillers, etc. The aspect ratio of the anisotropic filler is preferably 5.0 or more. The non-anisotropic filler includes spherical fillers, irregular fillers, etc.

[0053] The thermally conductive sheet 1 preferably contains a fibrous filler, a scaly filler, and a spherical filler as the thermally conductive filler, which makes it easier for the thermally conductive sheet 1 to satisfy the above-mentioned predetermined compressive load characteristics and thermal resistance value.

[0054] In this case, the content of the fibrous filler is preferably greater than the content of the scaly filler and the content of the spherical filler. In this case, it is easier to reduce the compressive load value while further increasing the thermal conductivity. On the other hand, if the content of the scaly filler is greater than the fibrous filler, it is difficult to reduce the compressive load value. If the content of the spherical filler is greater than the fibrous filler, it is difficult to increase the thermal conductivity.

[0055] The thermally conductive sheet 1 preferably contains carbon fibers 4C, scaly graphite powder 4G, and spherical zinc oxide particles 4Z as thermally conductive fillers. In this case, it is preferable that the carbon fibers 4C and graphite powder 4G are oriented substantially in the thickness direction of the thermally conductive sheet 1, and the zinc oxide particles 4Z are dispersed throughout the thermally conductive sheet 1. A thermally conductive sheet 1 having such a configuration is particularly suitable for increasing thermal conductivity while suppressing the initial load of the sheet-shaped thermally conductive composition.

[0056] The fiber length of the carbon fiber 4C is preferably 20 μm or more. If the fiber length is less than 20 μm, it may be difficult to form a heat conduction path, and the thermal conductivity of the thermal conductive sheet 1 may be poor. On the other hand, the upper limit of the fiber length of the carbon fiber 4C is preferably 500 μm from the viewpoint of ease of filling the thermal conductive sheet with the carbon fiber. The fiber length of the carbon fiber 4C is more preferably 50 μm or more and 300 μm or less.

[0057] The fiber diameter of the carbon fiber 4C is preferably 5 μm or more. If the fiber diameter is less than 5 μm, a heat conduction path is difficult to form, and the thermal conductivity of the thermal conductive sheet 1 may be poor. The preferred upper limit of the fiber diameter of the carbon fiber 4C is 20 μm from the viewpoint of processability when producing the thermal conductive sheet 1.

[0058] The fiber length of a fibrous filler such as carbon fiber refers to the arithmetic mean value of the length in the fiber direction determined using a microscopic image of the fibrous filler. The fiber diameter of a fibrous filler refers to the arithmetic mean value of the dimension in the radial direction determined using a microscopic image of the fibrous filler. The fiber length and fiber diameter are determined based on the measurement results obtained by acquiring a microscopic image of the fibrous filler, randomly selecting 20 fibrous fillers from the image, and measuring the length in the fiber direction and the dimension in the radial direction of the selected fibrous fillers.

[0059] The carbon fiber 4C may be one type of carbon fiber or two or more types of carbon fiber. Carbon fibers with different thermal conductivities may be used in combination as the carbon fiber 4C. When carbon fibers with high thermal conductivity are used, the thermal conductivity increases, but the initial compressive load required for 50% compressive deformation also tends to increase. Therefore, by using carbon fibers with different thermal conductivities in combination, it becomes easier to adjust the thermal conductivity and initial compressive load of the thermal conductive sheet 1.

[0060] The graphite powder 4G is preferably shaped like a scale. In this case, the graphite powder is oriented in the thickness direction of the thermally conductive sheet 1, which is suitable for increasing the thermal conductivity in the thickness direction. The graphite powder 4G may contain graphite powder in a shape other than a scale. Scale-shaped graphite powder and non-scale-shaped graphite powder may be used in combination.

[0061] The particle size of the flake graphite powder 4G is preferably 5 μm or more and 50 μm or less. If the particle size of the flake graphite powder 4G is less than 5 μm, it is difficult to form a heat conduction path within the thermal conductive sheet 1. On the other hand, if the particle size of the flake graphite powder 4G exceeds 50 μm, it is difficult to pack the powder densely. The particle size of the flake graphite powder 4G is preferably 10 μm or more and 30 μm or less.

[0062] The particle size of a scaly filler such as scaly graphite powder refers to the D50 (50% median diameter) of the maximum length in the plate surface direction obtained using a microscope image of the scaly filler for particle size measurement. The particle size is determined by obtaining a microscope image for particle size measurement of the scaly filler, randomly selecting 20 scaly fillers from the image, measuring the maximum length in the plate surface direction of the selected scaly fillers, and then based on the measurement results.

[0063] The zinc oxide particles 4Z are preferably spherical in shape, because in this case, the zinc oxide particles 4Z can be more easily filled into the thermal conductive sheet 1 than zinc oxide particles 4Z of other shapes, and the zinc oxide particles 4Z are less likely to damage components of the manufacturing equipment.

[0064] The particle size of the zinc oxide particles 4Z is preferably 0.1 μm or more and 10 μm or less. If the particle size of the zinc oxide particles 4Z is less than 0.1 μm, a heat conduction path is unlikely to be formed. On the other hand, if the particle size of the zinc oxide particles 4Z exceeds 10 μm, the orientation of the carbon fibers 4C and the scaly graphite powder 4G is likely to be hindered. Furthermore, the zinc oxide particles 4Z are likely to damage steel members of the manufacturing equipment.

[0065] In the embodiment of the present invention, the particle size of the thermally conductive filler other than the fibrous filler and the scaly filler refers to the value of the median diameter (d50) measured by a laser diffraction / scattering method.

[0066] When the thermally conductive filler 4 contains carbon fibers 4C, scaly graphite powder 4G, and spherical zinc oxide particles 4Z, the preferred content of the thermally conductive filler 4 in the thermally conductive sheet 1 is 50% by volume or more and 70% by volume or less, where the total content of the carbon fibers 4C, scaly graphite powder 4G, and spherical zinc oxide particles 4Z is less than 50% by volume. If the total content of the carbon fibers 4C, scaly graphite powder 4G, and spherical zinc oxide particles 4Z is less than 50% by volume, sufficient thermal conductivity may not be ensured. On the other hand, if the total content exceeds 70% by volume, the thermally conductive sheet 1 becomes too hard and may not be able to be properly attached to an IC chip with an allowable compression load. Furthermore, during the slicing process, which is one step in the manufacturing process of the thermally conductive sheet 1, cracks may occur in the sheet during molding, making it impossible to maintain the sheet shape. In the thermally conductive sheet 1, the total content of the carbon fibers 4C, the scaly graphite powder 4G, and the spherical zinc oxide particles 4Z is preferably 55% by volume or more and 70% by volume or less, which is more suitable for achieving both good thermal conductivity and appropriate hardness.

[0067] The content of carbon fiber 4C in thermally conductive sheet 1 is preferably 30% by volume or more and 45% by volume or less. This is suitable for ensuring good thermal conductivity of thermally conductive sheet 1. When the content of carbon fiber 4C in thermally conductive sheet 1 is 30% by volume or more and 45% by volume or less, the content of graphite powder 4G is preferably 5% by volume or more and 10% by volume or less. By setting the total content of the three types of thermally conductive fillers to 50% by volume or more and 70% by volume or less, and setting the contents of carbon fiber 4C and scaly graphite powder 4G within the above ranges, it is suitable for reducing the ratio of the compressive load value after 1 minute to the initial compressive load value while maintaining good thermal conductivity.

[0068] The total content of the scaly graphite powder 4G and spherical zinc oxide particles 4Z in the thermal conductive sheet 1 is preferably 20% by volume or more and 30% by volume or less. This is more suitable for reducing the compressive load required for 50% compressive deformation while maintaining good thermal conductivity. A more preferred content is 25% by volume or more and 30% by volume or less.

[0069] In the thermally conductive sheet 1, an example of a particularly suitable configuration of the thermally conductive filler 4 is, for example, a filler containing carbon fibers 4C, scaly graphite powder 4G, and spherical zinc oxide particles 4Z, wherein the total content of the carbon fibers 4C, scaly graphite powder 4G, and spherical zinc oxide particles 4Z is 50 volume % or more and 70 volume % or less, the content of the carbon fibers 4C is 30 volume % or more and 40 volume % or less, the content of the scaly graphite powder 4G is 5 volume % or more and 10 volume % or less, and the total content of the scaly graphite powder 4G and spherical zinc oxide particles 4Z is 25 volume % or more and 30 volume % or less.

[0070] Next, we will explain the method for producing the thermally conductive sheet 1. The thermally conductive sheet 1 can be produced, for example, by a first production method that involves the following steps (a) to (c): (a) preparing a silicone-based composition containing uncrosslinked silicone, carbon fiber, graphite powder, zinc oxide particles, and optional components such as a flame retardant and a coupling agent; (b) molding the prepared silicone-based composition; and (c) slicing the molded silicone-based composition into sheets.

[0071] First, step (a) is carried out to prepare a silicone composition. Here, the silicone composition is prepared by, for example, kneading uncrosslinked silicone, a thermally conductive filler (carbon fiber, graphite powder, and zinc oxide particles), and various additives as needed, using a twin roll mill. At this time, some or all of the components may be supplied as a compound.

[0072] Next, the prepared silicone composition is molded in step (b) and sliced ​​into sheets in step (c). The silicone composition can be molded, for example, using an extruder. Figure 3 shows a cross-sectional schematic diagram of the tip of an extruder and a T-die used in the manufacture of a thermally conductive sheet 1 according to an embodiment of the present invention. The silicone composition introduced into the extruder 30 is stirred and kneaded by a screw 34 and introduced into a first gap 32 of the T-die along a flow path 31.

[0073] The silicone-based composition stirred and kneaded in the extruder 30 is first squeezed in the vertical direction (thickness direction) by the first gap 32 to form a thin strip. At this time, the anisotropic thermally conductive filler mixed in the silicone-based composition is oriented in the flow direction (extrusion direction) of the silicone-based composition. Therefore, in the thin resin sheet 40 formed after passing through the first gap 32, the anisotropic thermally conductive filler is oriented in the plane direction of the resin sheet 40. In this embodiment, for example, carbon fiber or flaky graphite powder corresponds to the anisotropic thermally conductive filler.

[0074] When the thin resin sheet 40 in which the thermally conductive filler is oriented passes completely through the first gap 32, the flow direction of the sheet, which was limited to the extrusion direction, is released and the flow direction changes to a direction approximately perpendicular to the extrusion direction. After completely passing through the first gap 32, the resin sheet 40, whose flow direction has changed to a direction approximately perpendicular to the extrusion direction, is further extruded toward the second gap 33. As a result, the resin sheet 40, now approximately perpendicular to the extrusion direction, is folded and stacked in the second gap 33. At this time, most of the anisotropic thermally conductive filler (carbon fiber and flake graphite powder) is oriented in the plane direction of the resin sheet 40, so that the anisotropic thermally conductive filler in the resin sheet 40 stacked in the second gap 33 is oriented along the thickness direction (the vertical direction in FIG. 3 ).

[0075] Thus, in step (b), a silicone-based composition is extruded to form a resin sheet 40 in which the anisotropic thermally conductive filler is oriented in the extrusion direction, and then this resin sheet 40 is folded and stacked to form a block.

[0076] Then, in step (c), the block of laminated thin resin sheets 40 is sliced ​​in a direction perpendicular to the thickness direction. As a result, a thermally conductive sheet 1 having a predetermined thickness and in which the anisotropic thermally conductive filler is substantially oriented in the thickness direction can be obtained. Note that the block of resin sheet 40 produced in step (b) itself can also be used as a sheet-like thermally conductive sheet according to an embodiment of the present invention.

[0077] In the T-die, the depths of the first gap 32 and the second gap 33 (i.e., the dimensions of the first gap 32 and the second gap 33 in the direction perpendicular to the paper surface in FIG. 3 ) are substantially uniform throughout the T-die. Furthermore, the depth dimensions of the first gap and the second gap are not particularly limited, and various design changes are possible depending on the product width of the thermally conductive sheet 1 to be manufactured.

[0078] The method for manufacturing the thermally conductive sheet 1 is not limited to the first manufacturing method described above, but may be, for example, a second manufacturing method in which the following steps (d) to (f) are performed. Figures 4A to 4D are diagrams illustrating the second manufacturing method.

[0079] (d) preparing a silicone-based composition containing uncrosslinked silicone, carbon fiber, graphite powder, zinc oxide particles, and optional components such as a flame retardant and a coupling agent; (e) molding the prepared silicone-based composition; and (f) slicing the molded silicone-based composition into sheets.

[0080] First, step (d) is carried out to prepare a silicone-based composition. Here, for example, uncrosslinked silicone, thermally conductive filler (carbon fiber, graphite powder, and zinc oxide particles), and various additives added as needed are kneaded using a twin roll 51. The composition is then sheeted to produce a resin sheet 50 (see FIG. 4A). Some or all of the components may be compounded before supply.

[0081] Next, step (e) of molding the silicone-based composition is performed. In this step (e), resin sheets 50 made of the silicone-based composition are folded and stacked so that the resin sheets 50 are in close contact with each other (see FIG. 4A ). For example, by continuously supplying the resin sheets 50 onto a table 53 that periodically reciprocates, a laminate can be obtained in which the resin sheets 50 are stacked while being folded. At this time, the anisotropic thermally conductive filler is oriented in the plane direction of the resin sheets 50.

[0082] Thereafter, the folded portion of the resin sheet 50 is cut and removed using a cutter 54 (see FIG. 4B), resulting in a stack 55 of a plurality of resin sheets 50 that are not connected to one another.

[0083] Next, step (f) is performed in which the obtained laminate 55 is sliced ​​using a cutter 57 in a direction perpendicular to the surface of the resin sheet 50 (see FIG. 4C). This allows the thermally conductive sheet 1 to be obtained (see FIG. 4D). The thermally conductive sheet 1 can also be manufactured through such steps.

[0084] Hereinafter, the embodiments of the present invention will be described in more detail with reference to examples, but the embodiments of the present invention are not limited to the following examples.

[0085] The raw materials used in the examples and comparative examples are as follows: (Matrix components) Silicone A: polydimethylsiloxane with a mass average molecular weight of 140,000 Silicone B: vinyl group-containing compound (MR-53, manufactured by Dow Toray Industries, Inc.) Peroxide: (RC-4 50P FD, manufactured by Dow Toray Industries, Inc.) Silane coupling agent: octyltrimethoxysilane

[0086] (Thermal conductive filler) Carbon fiber A: K223HM (fibrous, fiber length: 200 μm / fiber diameter: 11 μm) manufactured by Mitsubishi Chemical Corporation Carbon fiber B: K23EHM (fibrous, fiber length: 200 μm / fiber diameter: 11 μm) manufactured by Mitsubishi Chemical Corporation Carbon fiber C: K223HM (fibrous, fiber length: 50 μm / fiber diameter: 11 μm) manufactured by Mitsubishi Chemical Corporation Graphite powder: CPB (flake, particle size: 22 μm) manufactured by Nippon Graphite Industries Co., Ltd. Zinc oxide particles: Zinc oxide type 1 (spherical, particle size: 0.8 μm) manufactured by Sakai Chemical Industry Co., Ltd. Alumina particles A: DAW-03 (spherical, particle size: 5 μm) manufactured by Denka Company Limited Alumina particles B: ASFP-09S (spherical, particle size: 1 μm) manufactured by Denka Company Limited Alumina particles C: AP10 (scale-shaped, particle size: 10 μm), manufactured by DIC Corporation. Magnesium hydroxide: EP-1A (spherical, particle size: 2 μm), manufactured by Konoshima Chemical Co., Ltd.

[0087] Example 1 In this example, a thermally conductive sheet 1 was manufactured using the second manufacturing method. 100 parts by mass of silicone A (polydimethylsiloxane with a mass average molecular weight of 140,000), 117 parts by mass of carbon fiber A, 60 parts by mass of carbon fiber B, 60 parts by mass of graphite powder, 304 parts by mass of zinc oxide particles, and 3.8 parts by mass of a silane coupling agent were kneaded using a two-roll mill 51 and then sheeted out to produce a resin sheet 50 made of a silicone-based composition with a thickness of approximately 1.0 to 1.2 mm. In this example, the volume fraction of carbon fiber A, carbon fiber B, graphite powder, and zinc oxide particles in the entire resin sheet 50 was 20% by volume, 10% by volume, 10% by volume, and 20% by volume, respectively, for a total volume fraction of the thermally conductive fillers of 60% by volume.

[0088] Next, the prepared resin sheets 50 are folded and stacked so that the sheets are in close contact with each other (see FIG. 4A ). At this time, the carbon fibers A and B and the graphite powder are oriented in the plane direction of the stacked resin sheets 50.

[0089] Next, the folded-back portions of the resin sheet 50 in the obtained laminate are cut and removed with a cutter 54. This results in a laminate 55 of multiple disconnected resin sheets 50 (see FIG. 4B). The laminate 55 is then sliced ​​in a direction perpendicular to the plane of the resin sheet 50 (see FIG. 4C), completing a 2 mm-thick thermally conductive sheet 1 in which the carbon fiber and graphite powder are oriented in the thickness direction (see FIG. 4D).

[0090] Example 2 A thermally conductive sheet was completed in the same manner as in Example 1, except that a resin sheet 50 made of a silicone-based composition and having a thickness of approximately 1.0 to 1.2 mm was prepared using the following method. 100 parts by mass of silicone A, 118 parts by mass of carbon fiber A, 60 parts by mass of carbon fiber B, 60 parts by mass of graphite powder, 305 parts by mass of zinc oxide particles, 4.0 parts by mass of silane coupling agent, and 16 parts by mass of magnesium hydroxide were kneaded using a two-roll mill 51 and then sheeted out to prepare a resin sheet 50 made of a silicone-based composition and having a thickness of approximately 1.0 to 1.2 mm. In this example, the volume fraction of carbon fiber A, carbon fiber B, graphite powder, zinc oxide particles, and magnesium hydroxide was 20% by volume, 10% by volume, 20% by volume, and 2.5% by volume, of the entire resin sheet 50, respectively, for a total volume fraction of the thermally conductive fillers of 62.5% by volume.

[0091] Example 3 A thermally conductive sheet was completed in the same manner as in Example 1, except that a resin sheet 50 made of a silicone-based composition and having a thickness of approximately 1.0 to 1.2 mm was prepared using the following method. 100 parts by mass of silicone A, 202 parts by mass of carbon fiber A, 67 parts by mass of carbon fiber B, 34 parts by mass of graphite powder, 348 parts by mass of zinc oxide particles, and 4.5 parts by mass of silane coupling agent were kneaded using a two-roll mill to prepare a resin sheet 50 having a thickness of approximately 1.0 to 1.2 mm. In this example, the volume fraction of carbon fiber A, the volume fraction of carbon fiber B, the volume fraction of graphite powder, the volume fraction of zinc oxide particles, and the volume fraction of zinc oxide particles were 30% by volume, 10% by volume, 5% by volume, and 20% by volume, respectively, of the entire resin sheet 50, and the total volume fraction of the thermally conductive fillers was 65% by volume.

[0092] Example 4 A thermally conductive sheet was completed in the same manner as in Example 1, except that a resin sheet 50 made of a silicone-based composition and having a thickness of approximately 1.0 to 1.2 mm was prepared using the following method. 100 parts by mass of silicone A, 232 parts by mass of carbon fiber A, 34 parts by mass of carbon fiber B, 66 parts by mass of graphite powder, 257 parts by mass of zinc oxide particles, and 3.5 parts by mass of silane coupling agent were kneaded using a two-roll mill to prepare a resin sheet 50 having a thickness of approximately 1.0 to 1.2 mm. In this example, the volume fraction of carbon fiber A, carbon fiber B, graphite powder, zinc oxide particles, and the total volume fraction of the thermally conductive fillers in the resin sheet 50 was 35% by volume, 5% by volume, 10% by volume, and 15% by volume, respectively.

[0093] Example 5 A thermally conductive sheet was completed in the same manner as in Example 1, except that a resin sheet 50 made of a silicone-based composition and having a thickness of approximately 1.0 to 1.2 mm was prepared by the following method. 100 parts by mass of silicone A, 90 parts by mass of carbon fiber A, 60 parts by mass of carbon fiber B, 60 parts by mass of graphite powder, 380 parts by mass of zinc oxide particles, and 4.5 parts by mass of a silane coupling agent were kneaded using a two-roll mill to prepare a resin sheet 50 having a thickness of approximately 1.0 to 1.2 mm. In this example, the volume fraction of carbon fiber A, the volume fraction of carbon fiber B, the volume fraction of graphite powder, and the volume fraction of zinc oxide particles were 15% by volume, 10% by volume, and 25% by volume, respectively, of the entire resin sheet 50, and the total volume fraction of the thermally conductive fillers was 60% by volume.

[0094] Example 6 A thermally conductive sheet was completed in the same manner as in Example 1, except that a resin sheet 50 made of a silicone-based composition and having a thickness of approximately 1.0 to 1.2 mm was prepared by the following method. 100 parts by mass of silicone A, 137 parts by mass of carbon fiber A, 45 parts by mass of carbon fiber B, 142 parts by mass of zinc oxide particles, and 2.0 parts by mass of a silane coupling agent were kneaded using a two-roll mill to prepare a resin sheet 50 having a thickness of approximately 1.0 to 1.2 mm. In this example, the volume fraction of carbon fiber A, the volume fraction of carbon fiber B, and the volume fraction of zinc oxide particles were 37.5% by volume, 12.5% ​​by volume, and 15% by volume, respectively, of the entire resin sheet 50, respectively, and the total volume fraction of the thermally conductive fillers was 65% by volume.

[0095] Example 7 A thermally conductive sheet was completed in the same manner as in Example 1, except that a resin sheet 50 made of a silicone-based composition and having a thickness of approximately 1.0 to 1.2 mm was prepared by the following method. 100 parts by mass of silicone A, 355 parts by mass of carbon fiber A, 40 parts by mass of graphite powder, 410 parts by mass of zinc oxide particles, and 5.0 parts by mass of a silane coupling agent were kneaded using a twin roll 51 and then sheeted out to prepare a resin sheet 50 made of a silicone-based composition and having a thickness of approximately 1.0 to 1.2 mm. In this example, the volume fraction of carbon fiber A, the volume fraction of graphite powder, and the volume fraction of zinc oxide particles were 45% by volume, 5% by volume, and 20% by volume, respectively, of the entire resin sheet 50, respectively, and the total volume fraction of the thermally conductive fillers was 70% by volume.

[0096] Comparative Example 1 A thermally conductive sheet was completed in the same manner as in Example 1, except that a resin sheet 50 made of a silicone-based composition and having a thickness of approximately 1.0 to 1.2 mm was prepared by the following method. 100 parts by mass of silicone A, 135 parts by mass of carbon fiber A, 45 parts by mass of carbon fiber B, 185 parts by mass of zinc oxide particles, and 2.0 parts by mass of a silane coupling agent were kneaded using a two-roll mill to prepare a resin sheet 50 having a thickness of approximately 1.0 to 1.2 mm. In this example, the volume fraction of carbon fiber A, the volume fraction of carbon fiber B, and the volume fraction of zinc oxide particles were 37.5% by volume, 12.5% ​​by volume, and 20% by volume, respectively, of the entire resin sheet 50, respectively, and the total volume fraction of the thermally conductive fillers was 70% by volume.

[0097] Comparative Example 2 A thermally conductive sheet was completed in the same manner as in Example 1, except that a resin sheet 50 made of a silicone-based composition and having a thickness of approximately 1.0 to 1.2 mm was prepared using the following method. 100 parts by mass of silicone A, 335 parts by mass of carbon fiber A, 25 parts by mass of graphite powder, 320 parts by mass of alumina particles A, 105 parts by mass of alumina particles B, and 2.5 parts by mass of a silane coupling agent were kneaded using a two-roll mill to prepare a resin sheet 50 having a thickness of approximately 1.0 to 1.2 mm. In this example, the volume fraction of carbon fiber A relative to the entire resin sheet 50 was 40% by volume, the volume fraction of graphite powder was 3% by volume, the volume fraction of alumina particles A was 22.5% by volume, and the volume fraction of alumina particles B was 7.5% by volume, resulting in a total volume fraction of the thermally conductive fillers of 73% by volume.

[0098] Comparative Example 3 A thermally conductive sheet was completed in the same manner as in Example 1, except that a resin sheet 50 made of a silicone-based composition and having a thickness of approximately 1.0 to 1.2 mm was prepared by the following method. 110 parts by mass of silicone A, 87 parts by mass of graphite powder, 190 parts by mass of alumina particles B, and 2.0 parts by mass of a silane coupling agent were kneaded using a two-roll mill to prepare a resin sheet 50 having a thickness of approximately 1.0 to 1.2 mm. In this example, the volume fraction of the graphite powder and the volume fraction of the alumina particles B relative to the entire resin sheet 50 were 27% by volume, 36% by volume, and the total volume fraction of the thermally conductive filler was 63% by volume.

[0099] Comparative Example 4 A thermally conductive sheet was completed in the same manner as in Example 1, except that a resin sheet 50 made of a silicone-based composition and having a thickness of approximately 1.0 to 1.2 mm was prepared by the following method. 100 parts by weight of silicone A, 1.6 parts by weight of silicone B, 0.7 parts by weight of peroxide, 180 parts by weight of carbon fiber C, and 80 parts by weight of alumina particles C were kneaded using a two-roll mill to prepare a resin sheet 50 having a thickness of approximately 1.0 to 1.2 mm. In this example, the volume fraction of carbon fiber C relative to the entire resin sheet 50 was 40% by volume, the volume fraction of alumina particles C was 10% by volume, and the total volume fraction of the thermally conductive filler was 50% by volume.

[0100] [Evaluation Test] (1) Load Value at 50% Compression The thermally conductive sheets prepared in the Examples and Comparative Examples were further cut to prepare disc-shaped evaluation samples with a diameter of 12 mm and a thickness of 2 mm. Using an Instron 5969 (manufactured by Instron) as a measuring instrument, the sheet was compressed at a compression rate of 5 mm / min to a thickness of "thickness before measurement x 0.5" (50% compression), and the load value at that time (N / 113 mm 2 The initial load value was measured. The compressed state was maintained for 1 minute, and the load value (N / 113 mm 2 ) was measured. The results are shown in Table 1. In addition, the ratio of the load value after 1 minute to the initial load value was calculated. The results are shown in Table 1.

[0101] (2) Thermal Resistance at 20% Compression The thermally conductive sheets prepared in the Examples and Comparative Examples were further cut to prepare evaluation samples with a diameter of 33 mm and a thickness of 2 mm. Using a TIMtester 1400 (manufactured by AnalysisTech) as a measuring device, the sheet was compressed to a thickness of "thickness before measurement x 0.8" (20% compression), and the thermal resistance was measured in that state. The sample temperature during measurement was 25°C. The results are shown in Table 1.

[0102] (3) Conformability: Figures 5A to 5C are diagrams illustrating the method for evaluating conformability. The thermally conductive sheets produced in the examples and comparative examples were further cut to produce evaluation samples 71 measuring 40 mm in length, 40 mm in width, and 2 mm in thickness. The conformability of these evaluation samples 71 was evaluated using the following method. The results are shown in Table 1. The evaluation sample 71 was placed on a lower glass plate 72. An aluminum plate 75 measuring 10 mm in length, 10 mm in width, and 1 mm in thickness was placed in the center of the top surface of the evaluation sample 71. An upper glass plate 73 was then placed on top of the aluminum plate 75 (see Figure 5A). In this state, a downward load was applied to the upper glass plate 73, and the upper glass plate 73 was moved at a speed of 5 mm / min until the gap between the top surface of the lower glass plate 72 and the bottom surface of the upper glass plate 73 became 2 mm. This caused the aluminum plate 75 to be pressed into the evaluation sample 71 (see Figures 5B and 5C). As a result, depressions 77 are formed along the outer edge of aluminum plate 75. In this state, the width W of the opening of depression 77 formed on the outer edge of aluminum plate 75 (see FIG. 5C) is measured on each side of aluminum plate 75 using a microscope. Based on the measured values, the followability is evaluated according to the following criteria. FIG. 5C is an enlarged view of the vicinity of region A in FIG. 5B. ◯: The maximum width of the opening was less than 1000 μm. ×: The maximum width of the opening was 1000 μm or more.

[0103]

[0104] The embodiments disclosed herein should be considered to be illustrative in all respects and not restrictive. The scope of the present invention is defined by the claims, and it is intended to include all modifications within the meaning and scope of the claims.

[0105] REFERENCE SIGNS LIST 1 Thermally conductive sheet (sheet-shaped thermally conductive composition) 2 Matrix component 4 Thermally conductive filler 4C Carbon fiber 4G Graphite powder 4Z Zinc oxide powder 11 IC chip 12 Heat sink 30 Extruder 31 Flow path 32 First gap 33 Second gap 34 Screw 40, 50 Resin sheet 51, 52 53 Table 54, 57 Cutter 55 Laminate 71 Evaluation sample 72 Lower glass plate 73 Upper glass plate 75 Aluminum plate 77 Recess

Claims

1. A sheet-shaped thermally conductive composition made of a resin composition containing silicone and a thermally conductive filler, which has an initial compression load value of 1.0 N / mm when compressed by 50%. 2 a ratio of a compressive load value after 1 minute to the initial compressive load value is 0.5 or less, and an apparent thermal conductivity when compressed and deformed by 20% is 22.8 W / mK or more.

2. The compressive load value after the one minute period is 0.4 N / mm 2 2. The thermally conductive composition of claim 1, wherein:

3. The thermally conductive composition according to claim 1 or 2, wherein the resin composition contains polydimethylsiloxane as the silicone.

4. A thermally conductive composition according to any one of claims 1 to 3, wherein the resin composition contains, as the thermally conductive filler, an anisotropic thermally conductive filler and a non-anisotropic thermally conductive filler.

5. A thermally conductive composition according to any one of claims 1 to 4, wherein the resin composition contains, as the thermally conductive fillers, a fibrous filler, a scaly filler, and a spherical filler.

6. A thermally conductive composition according to any one of claims 1 to 5, wherein the resin composition contains, as thermally conductive fillers, carbon fibers, flake graphite powder, and spherical zinc oxide particles.

7. The thermally conductive composition according to claim 6, wherein the total content of the carbon fibers, the scaly graphite powder, and the spherical zinc oxide particles in the thermally conductive composition is 50 volume % or more and 70 volume % or less.

8. The thermally conductive composition according to claim 6 or 7, wherein the content of the carbon fiber in the thermally conductive composition is 30 volume % or more and 45 volume % or less.

Citation Information

Patent Citations

  • Heat dissipating member

    JP2005072220A

  • Resin composition

    JP2009197052A

  • Thermal conductive sheet

    JP2010007039A

  • Anisotropic thermal conductive sheet having self-adhesiveness

    JP2020176182A

  • Thermally conductive sheet and method for manufacturing thermally conductive sheet

    JP2022037609A