Composite and production method therefor

The composite addresses the handling issues of boron nitride sintered bodies by selectively filling pores with resin, reducing weight and enhancing handling, while maintaining thermal and corrosion resistance through a method of impregnation and curing, effectively preventing damage and improving mechanical strength.

WO2024204446A1PCT designated stage expired Publication Date: 2024-10-03DENKA CO LTD

Patent Information

Application Number
PCT/JP2024/012466
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Boron nitride sintered bodies are prone to chipping and cracking due to their porosity and difficulty in handling when filled with resin, which increases weight and impairs handling properties.

Method used

A composite comprising a porous boron nitride sintered body with selectively filled and unfilled pores, where the unfilled pores reduce weight and enhance handling, and a method involving impregnation and curing of resin in the surface pores to form a composite with a resin-filled and resin-free interior.

Benefits of technology

The composite achieves improved handling properties by reducing weight and preventing damage from external forces while maintaining thermal conductivity and corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012466_03102024_PF_FP_ABST
    Figure JP2024012466_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This composite comprises: a porous sintered boron nitride product; and a resin with which some of the pores of the sintered boron nitride product are filled. The sintered boron nitride product has: a filled portion where the pores are filled with the resin; and an unfilled portion which is surrounded by the filled portion and in which the pores are unfilled with a resin. This method for producing a composite comprises: an impregnation step in which pores in a surface portion of a porous sintered boron nitride product are impregnated with a resin composition to obtain a resin-impregnated object; and a curing step in which the resin-impregnated object is heated to cure the resin composition, thereby forming a filled portion where the pores are filled with the resin and an unfilled portion which is surrounded by the filled portion and in which the pores are unfilled with a resin.
Need to check novelty before this filing date? Find Prior Art

Description

Composite and manufacturing method thereof

[0001] The present disclosure relates to composites and methods for making the same.

[0002] Boron nitride has excellent heat resistance, thermal conductivity, corrosion resistance, and processability. For these reasons, it is used in a variety of applications. In recent years, attempts have been made to combine resins with boron nitride sintered bodies to further improve the inherent properties of boron nitride and to impart new properties such as adhesiveness. For example, Patent Document 1 proposes a composite that can flexibly accommodate prioritized properties by varying the cure rate of the resin at the surface and in the interior of the composite.

[0003] International Publication No. 2022 / 209971

[0004] Boron nitride is a ceramic material that is difficult to sinter, and therefore has many pores inside when a sintered body is formed by a powder metallurgy process. Therefore, when an external force is applied, the corners may chip or crack. To prevent such damage, it is considered effective to fill the boron nitride sintered body with resin, as in Patent Document 1. However, filling the boron nitride sintered body with resin increases its weight, impairing its handleability. Therefore, the present disclosure provides a composite body with excellent handleability and a method for producing the same.

[0005] One aspect of the present disclosure provides the following conjugate:

[0006] [1] A composite comprising a porous boron nitride sintered body and a resin filled into some of the pores of the boron nitride sintered body, wherein the boron nitride sintered body has a filled portion where the pores are filled with the resin, and an unfilled portion surrounded by the filled portion where the pores are not filled with the resin.

[0007] The boron nitride sintered body in the composite of [1] above has unfilled portions in which the pores are not filled with resin, thereby enabling the weight of the composite to be reduced. The boron nitride sintered body in the composite of [1] above has filled portions in which the pores are filled with resin. Therefore, even if the composite is grasped using, for example, a robot or a jig, or if the composite is dropped, damage to the composite can be sufficiently suppressed. Therefore, the composite has excellent handleability.

[0008] The composite of [1] above may be any one of [2] to [8] below. [2] The composite of [1], further comprising a resin layer covering at least a portion of the filled portion. [3] The composite of [1] or [2], wherein the porosity of the boron nitride sintered body is 56% by volume or less. [4] The composite of [1] to [3], wherein the average pore size of the pores in the boron nitride sintered body is 1.5 μm or less. [5] The composite of [1] to [4], wherein the filled portion in the boron nitride sintered body has an edge that protrudes outward. [6] The composite of [1] to [5], wherein the boron nitride sintered body is plate-shaped and has a thickness of 30 mm or more. [7] The composite of [1] to [6], wherein the ratio of the cross-sectional area N of the unfilled portion to the cross-sectional area W of the boron nitride sintered body is 0.2 or more. [8] The composite of [1] to [7], wherein the volume of the unfilled portion is larger than the volume of the filled portion.

[0009] One aspect of the present disclosure provides the following method for producing a composite: [9] A method for producing a composite, comprising: an impregnation step of impregnating pores in the surface portion of a porous boron nitride sintered body with a resin composition to obtain a resin-impregnated body; and a curing step of heating the resin-impregnated body to cure the resin composition and form a filled portion in which the pores are filled with resin and an unfilled portion surrounded by the filled portion and in which the pores are not filled with resin.

[0010] The composite obtained by the manufacturing method [9] above includes a boron nitride sintered body having unfilled portions where the pores are not filled with resin, thereby enabling the weight of the composite to be reduced. The boron nitride sintered body in the composite obtained by the manufacturing method [9] above has filled portions where the pores are filled with resin. Therefore, even if the composite is grasped using a robot or jig, or if the composite is dropped, damage to the composite can be sufficiently suppressed. Therefore, the composite obtained by the above manufacturing method has excellent handleability.

[0011] The method for producing a composite according to the above item [9] may be the following item

[10] :

[10] The method for producing a composite according to item [9], wherein the porosity of the boron nitride sintered body is 56% by volume or less, and the average pore size of the pores is 1.5 μm or less.

[0012] According to the present disclosure, it is possible to provide a composite that is easy to handle and a method for producing the same.

[0013] Fig. 1 is a cross-sectional view showing an example of a composite; Fig. 2 is a cross-sectional photograph of another example of a composite; Fig. 3 is a perspective view of a boron nitride sintered body used in the examples; Fig. 4(A) is a photograph showing a cross-section of the composite of Example 3, and Fig. 4(B) is a photograph showing a cross-section of the composite of Comparative Example 1.

[0014] Hereinafter, several embodiments of the present disclosure will be described, with reference to the drawings where necessary. However, the following embodiments are merely examples for explaining the present disclosure and are not intended to limit the present disclosure to the following content. Each numerical range indicated with the symbol "to" includes both the lower and upper limits. That is, a numerical range indicated as "A to B" means A or more and B or less. The present disclosure also includes a case in which the upper or lower limit of each numerical range is replaced with the numerical value of any of the examples. When multiple materials are exemplified, one of the materials may be used alone, or multiple materials may be used in combination.

[0015] A composite according to one embodiment comprises a porous boron nitride sintered body and a resin filled into some of the pores of the boron nitride sintered body. The boron nitride sintered body has a filled portion in which the pores are filled with the resin and an unfilled portion surrounded by the filled portion in which the pores are not filled with the resin. The pores in the unfilled portion are voids.

[0016] A boron nitride sintered body is obtained by firing a compact formed under pressure, or by firing while forming under pressure (e.g., hot pressing). Aggregates and lumps obtained by firing boron nitride powder without molding are not considered boron nitride sintered bodies. A boron nitride sintered body contains boron nitride particles formed by sintering primary particles of boron nitride together, and pores. The pores may include open pores and closed pores, or may include only open pores. A resin is filled in some of the open pores. The average pore diameter of the pores in the boron nitride sintered body may be 1.5 μm or less, 1.0 μm or less, or 0.6 μm or less. The small pore size of such a boron nitride sintered body further suppresses the occurrence of cracks and chips in the boron nitride sintered body. Furthermore, the impregnation of the resin composition into the interior can be sufficiently suppressed. Furthermore, the contact area between boron nitride particles is increased, thereby increasing thermal conductivity. The average pore size of the pores in the boron nitride sintered body may be 0.1 μm or more, 0.2 μm or more, or 0.3 μm or more. Such a boron nitride sintered body allows for smooth formation of a filling portion on its surface. An example of the range of the average pore size may be 0.1 to 1.5 μm.

[0017] The average pore size of the pores in a boron nitride sintered body can be measured by the following procedure. First, the composite is heated to remove the resin from the filled portion to obtain a boron nitride sintered body. If a boron nitride sintered body before being filled with resin is available, that boron nitride sintered body may be used. Using a mercury porosimeter, the pore size distribution is determined when the boron nitride sintered body is pressurized while increasing the pressure from 0.0042 MPa to 206.8 MPa. With the pore size on the horizontal axis and the cumulative pore volume on the vertical axis, the pore size at which the cumulative pore volume reaches 50% of the total pore volume is the average pore size. Mercury porosimeters manufactured by Shimadzu Corporation can be used. The average pore size in this specification is a value determined for not only pores not filled with resin, but also pores filled with resin.

[0018] The porosity of the boron nitride sintered body, i.e., the ratio of the volume of pores in the boron nitride sintered body, may be 56 vol% or less, 50 vol% or less, 45 vol% or less, 40 vol% or less, 35 vol% or less, or 30 vol% or less. This makes it possible to prevent the resin composition from penetrating into the interior of the boron nitride sintered body when the boron nitride sintered body is impregnated with the resin composition. The porosity of the boron nitride sintered body may be 10 vol% or more, or 15 vol% or more. This makes it possible to smoothly form a filled portion on the surface of the boron nitride sintered body. An example of the range of the porosity of the boron nitride sintered body is 10 to 56 vol%. In this specification, the porosity refers to the total volume ratio of pores filled with resin and pores not filled with resin to the volume of the boron nitride sintered body.

[0019] The porosity was calculated from the volume and weight of the boron nitride sintered body by calculating the bulk density [B (g / cm 3 )] was calculated, and the bulk density was compared with the theoretical density of boron nitride [A (g / cm 3 The theoretical density A of the boron nitride sintered body is 2.26 g / cm 3 Porosity (volume%) = [1 - (B / A)] x 100 (1)

[0020] The bulk density B of the boron nitride sintered body is 1.0 g / cm 3 Above, 1.1g / cm 3 Above, 1.2g / cm 3 or more, or 1.5 g / cm 3 A boron nitride sintered body having a large bulk density B can suppress the occurrence of cracks and chips. The bulk density B of the boron nitride sintered body is 2.1 g / cm 3 or less, or 2.0 g / cm 3 This allows the filling portion to be smoothly formed on the surface of the boron nitride sintered body. An example of the range of the bulk density B of the boron nitride sintered body is 1.0 to 2.1 g / cm 3 is.

[0021] The resin contained in the composite may be a cured product of a resin composition containing a base agent and a curing agent. The cured product in this specification may be either a fully cured (C stage) or semi-cured (B stage) product. The resin in this specification may also be a fully cured product or a semi-cured product. "Completely cured" means that the curing reaction of the resin composition has progressed completely. "Semi-cured" means that the curing reaction of the resin composition has progressed partially. The resin may include a thermosetting resin or the like produced by the reaction of the base agent and curing agent in the resin composition, and may include monomers such as the base agent and curing agent.

[0022] The resin may include at least one selected from the group consisting of epoxy resin, silicone resin, cyanate resin, silicone rubber, acrylic resin, phenolic resin, melamine resin, urea resin, bismaleimide resin, unsaturated polyester, fluororesin, polyimide, polyamideimide, polyetherimide, polybutylene terephthalate, polyethylene terephthalate, polyphenylene ether, polyphenylene sulfide, wholly aromatic polyester, polysulfone, liquid crystal polymer, polyethersulfone, polycarbonate, maleimide resin, maleimide-modified resin, ABS (acrylonitrile-butadiene-styrene) resin, AAS (acrylonitrile-acrylic rubber-styrene) resin, AES (acrylonitrile-ethylene-propylene-diene rubber-styrene) resin, polyglycolic acid resin, polyphthalamide, and polyacetal. One of these may be used alone, or two or more may be used in combination.

[0023] The weight ratio of the resin in the composite may be less than 45 wt %, 35 wt % or less, 25 wt % or less, or 15 wt % or less, based on the total weight of the composite. This allows the weight of the composite to be sufficiently lightened, further improving handleability. Furthermore, the resin can be easily removed from the composite. Therefore, when in use, the resin can be removed and the composite can be used smoothly as a resin-free boron nitride sintered body. This weight ratio can be adjusted by changing the density of the impregnated resin or by changing the filling rate of the pores in the boron nitride sintered body.

[0024] The weight ratio of the resin in the composite may be 3 wt% or more, or 10 wt% or more, based on the total weight of the composite. This can sufficiently suppress damage such as cracking and chipping of the boron nitride sintered body. The weight ratio of the resin in the composite may range from 3 wt% or more to less than 45 wt%. The shape of the composite is not particularly limited, and may be, for example, a block or plate shape. The thickness of the composite may be 20 mm or more, or 30 mm or more. By increasing the thickness, the volume of the non-filled portion can be sufficiently increased.

[0025] The thickness of the composite is measured in a direction perpendicular to the main surface. If the thickness of the composite is not constant, the thickness is measured at 10 selected locations, and the average value is within the above-mentioned range. There is no particular limitation on the size of the main surface of the composite. The main surface of the composite may be, for example, 50 mm 2 It may be 200 mm or more, 2 It may be 1000 mm or more, 2 It may be more than that.

[0026] An example of a cross section of a composite according to the above embodiment is shown in Figure 1. The composite 100 in Figure 1 may be in the shape of a block or a plate. The composite 100 comprises a boron nitride sintered body 10 and a resin layer 20 covering the entire surface of the boron nitride sintered body 10. The boron nitride sintered body 10 has an unfilled portion 12 in its interior (central portion) where the pores are not filled with resin, and a filled portion 14 on the surface surrounding the unfilled portion 12 where the pores are filled with resin. The filled portion 14 is provided so as to surround the unfilled portion 12. All of the pores in the unfilled portion 12 are voids.

[0027] In the filled portion 14, not all pores need to be filled with resin. For example, closed pores in the filled portion 14 do not need to be filled with resin. The boundary 13 between the filled portion 14 and the unfilled portion 12 is drawn by connecting adjacent pores that are filled with resin and are located near the center of the boron nitride sintered body with a line. In a cross-sectional view such as Figure 1, the outline of the filled portion 14 and the outline of the boron nitride sintered body 10 may or may not be similar.

[0028] The filling portion 14 has an edge 14e that protrudes outward. The edge of a boron nitride sintered body that is not filled with resin is more susceptible to damage such as cracks and chips than other portions. However, since the pores of the filling portion 14 are filled with resin, damage such as cracks and chips can be sufficiently suppressed even at the edge 14e. For example, even if a gripping part of a robot or the like collides with the edge 14e or grips the edge 14e too tightly, damage can be sufficiently suppressed. In this specification, edges include corners and ridges.

[0029] In a cross section such as that shown in FIG. 1 , the ratio (N / W) of the cross-sectional area N of the unfilled portion 12 to the cross-sectional area W of the boron nitride sintered body 10 may be 0.2 or greater, 0.3 or greater, 0.4 or greater, or 0.5 or greater. Increasing the ratio (N / W) can further reduce the weight of the composite 100. Furthermore, resin can be removed from the composite 100 to obtain a resin-free boron nitride sintered body 10 smoothly and efficiently. The ratio (N / W) may be 0.7 or less. This sufficiently prevents damage to the boron nitride sintered body 10, such as cracking and chipping. The ratio (N / W) is a value measured at the cross section of the boron nitride sintered body 10 where the ratio (N / W) is greatest. The ratio (N / W) may be, for example, 0.2 to 0.7.

[0030] The volume ratio of the non-filled portions 12 to the entire boron nitride sintered body 10 may be 0.2 or more, 0.3 or more, or 0.4 or more. This allows the weight of the composite 100 to be reduced. Furthermore, the resin can be removed from the composite 100 to smoothly obtain a resin-free boron nitride sintered body 10. From the same perspective, the volume of the non-filled portions 12 may be larger than the volume of the filled portions 14. The volume ratio of the non-filled portions 12 to the entire boron nitride sintered body 10 may be 0.8 or less. This allows the boron nitride sintered body 10 to be sufficiently prevented from being damaged, such as cracked or chipped.

[0031] The resin layer 20 may have the same components as the resin filled in the filling portion 14. By providing the resin layer 20, damage such as cracking and chipping of the boron nitride sintered body 10 can be further suppressed. The thickness of the resin layer 20 may be 0.1 mm or more, 0.5 mm or more, or 1.0 mm or more. This sufficiently suppresses damage such as cracking and chipping of the boron nitride sintered body 10. The thickness of the resin layer 20 may be 5 mm or less, or 3 mm or less. This facilitates smooth removal of the resin layer 20 from the composite body 100. Furthermore, the weight of the composite body 100 can be reduced. As shown in FIG. 1 , the resin layer 20 does not necessarily cover the entire surface of the boron nitride sintered body 10, and may cover only a portion of the surface of the boron nitride sintered body 10. For example, the resin layer may be provided so as to cover only the outwardly protruding edge 14e and its vicinity. This efficiently protects the vulnerable parts.

[0032] Figure 2 is a photograph showing the cross section of another example of a composite. Composite 100A includes a boron nitride sintered body 10A having a rectangular cross section as shown in Figure 2. Composite 100A in Figure 2 is cut along a direction perpendicular to its thickness direction and passing through the center of composite 100A. Boron nitride sintered body 10A has an unfilled portion 12 in which the pores are not filled with resin, and a filled portion 14 in which the pores are filled with resin and formed to surround unfilled portion 12. Composite 100A has a resin layer 20 covering filled portion 14. It should be noted that the presence of resin layer 20 is not essential, and filled portion 14 may be exposed on the surface.

[0033] Because composites 100 and 100A have non-filled portions 12, their weight can be reduced compared to composites without non-filled portions 12. Because boron nitride sintered bodies 10 and 10A have filled portions 14 that completely surround non-filled portions 12, damage to boron nitride sintered bodies 10 and 10A can be sufficiently suppressed. This allows them to be smoothly gripped by a robot or jig. Therefore, composites 100 and 100A are easy to handle. Because composites 100 and 100A have filled portions 14, they can suppress moisture penetration into the pores of non-filled portions 12 even when stored in a high-humidity environment for a long period of time. Therefore, when used in an environment exposed to high temperatures after long-term storage, moisture condensed in the pores can be prevented from boiling off, preventing damage to the composite. One such application is a protective component for a thermometer that measures the temperature inside a plant, such as a blast furnace.

[0034] A method for producing a composite according to one embodiment includes an impregnation step in which pores in the surface of a porous boron nitride sintered body are impregnated with a resin composition to obtain a resin-impregnated body, and a curing step in which the resin-impregnated body is heated to cure the resin composition, thereby forming a filled portion in which the pores are filled with resin in the surface portion and an unfilled portion in which the pores inside the boron nitride sintered body are not filled with resin. The following describes the production of the composite 100 shown in Figure 1 as an example.

[0035] Porous boron nitride sintered bodies can be obtained by the following sintering process. First, a raw material powder containing boron nitride is prepared. The raw material powder may contain, in addition to boron nitride, at least one nitride selected from the group consisting of aluminum nitride and silicon nitride. The boron nitride may be amorphous boron nitride or hexagonal boron nitride. When preparing a boron nitride sintered body, for example, amorphous boron nitride powder having an average particle size of 0.5 to 10 μm or hexagonal boron nitride powder having an average particle size of 3.0 to 40 μm can be used as the raw material powder.

[0036] In the sintering step, a compound containing boron nitride powder may be molded and sintered to obtain a boron nitride sintered body. The molding may be performed by uniaxial pressing or cold isostatic pressing (CIP). A sintering aid may be added to the compound before molding to obtain the compound. Examples of sintering aids include metal oxides such as yttria oxide, aluminum oxide, and magnesium oxide, alkali metal carbonates such as lithium carbonate and sodium carbonate, and boric acid. When a sintering aid is added, the amount of the sintering aid may be, for example, 0.01 parts by weight or more, or 0.1 parts by weight or more, per 100 parts by weight of the total of the boron nitride powder and the sintering aid. The amount of the sintering aid may be, for example, 20 parts by weight or less, 15 parts by weight or less, or 10 parts by weight or less, per 100 parts by weight of the total of the boron nitride powder and the sintering aid.

[0037] The compound may be formed into a block or plate-shaped compact by, for example, a slip casting method. The molding method is not particularly limited, and examples include press molding using a mold and cold isostatic pressing (CIP). The molding pressure may be, for example, 20 to 500 MPa. Increasing the molding pressure can reduce the average pore size and porosity of the boron nitride sintered body and increase the bulk density. In order to sufficiently increase the volume ratio and cross-sectional area ratio (N / W) of the unfilled portion, the thickness of the compact may be 30 mm or more, 40 mm or more, or 50 mm or more. The thickness of the compact is measured in a direction perpendicular to the main surface. If the thickness of the compact is not constant, the thickness is measured at 10 randomly selected locations, and the average value is within the above-mentioned range.

[0038] The sintering temperature in the sintering step may be, for example, 1600°C or higher, or 1700°C or higher. The sintering temperature may be, for example, 2200°C or lower, or 2000°C or lower. The sintering time may be, for example, 10 hours or shorter, or 5 hours or shorter. By shortening the sintering time, the average pore size and porosity of the boron nitride sintered body can be reduced, and the bulk density can be increased. Note that a first firing may be performed at a temperature lower than the above sintering temperature, and then a second firing may be performed at the above sintering temperature. The sintering atmosphere may be, for example, an inert gas atmosphere such as nitrogen, helium, or argon. By setting the amount of sintering aid added within the above range, it becomes easier to adjust the average pore size of the boron nitride sintered body to the above range.

[0039] For sintering, for example, a batch furnace or a continuous furnace can be used. Examples of batch furnaces include muffle furnaces, tubular furnaces, and atmosphere furnaces. Examples of continuous furnaces include rotary kilns, screw conveyor furnaces, tunnel furnaces, belt furnaces, pusher furnaces, and large continuous furnaces. In this way, a boron nitride sintered body can be obtained. The boron nitride sintered body may be block-shaped or plate-shaped. The thickness of the boron nitride sintered body may be 30 mm or more, 40 mm or more, or 50 mm or more. The thickness of the boron nitride sintered body is measured in a direction perpendicular to the main surface. If the thickness of the boron nitride sintered body is not constant, the thickness may be measured at 10 randomly selected locations, and the average value may be within the above-mentioned range.

[0040] In the impregnation step, the resin composition is impregnated into the pores in the surface portion of the boron nitride sintered body to obtain a resin-impregnated body. At this time, the resin composition is impregnated only into the surface portion of the boron nitride sintered body, and the resin composition is prevented from impregnating the pores inside the boron nitride sintered body. For this reason, it is preferable to increase the viscosity of the resin composition within a range that allows for easy handling. The viscosity of the resin composition when impregnating the boron nitride sintered body may be, for example, greater than 1000 mPa·s. The resin composition may also be impregnated into the pores in the surface portion of the boron nitride sintered body without heating.

[0041] The impregnation of the resin composition into the boron nitride sintered body may be carried out under normal pressure or under reduced pressure without applying pressure. This can prevent the resin composition from penetrating into the interior of the boron nitride sintered body. The impregnation time may be adjusted to control the amount of resin composition impregnated. When impregnation is carried out under pressure using an impregnation device, the impregnation time may be shortened to prevent the resin composition from penetrating into the interior of the boron nitride sintered body. When impregnation is carried out under pressure to prevent the resin composition from penetrating into the interior of the boron nitride sintered body, the pressure may be less than 1 MPa. The impregnation may be carried out by immersing the boron nitride sintered body in the resin composition. However, instead of immersing the entire boron nitride sintered body in the resin composition, for example, only the lower part may be immersed to prevent the resin composition from penetrating into the interior of the boron nitride sintered body.

[0042] The resin composition can be, for example, one that becomes the resin described in the description of the composite through a curing reaction. The resin composition may contain a solvent. The viscosity of the resin composition may be adjusted by changing the amount of solvent added, or by partially progressing the curing reaction. Examples of solvents include aliphatic alcohols such as ethanol and isopropanol; ether alcohols such as 2-methoxyethanol, 1-methoxyethanol, 2-ethoxyethanol, 1-ethoxy-2-propanol, 2-butoxyethanol, 2-(2-methoxyethoxy)ethanol, 2-(2-ethoxyethoxy)ethanol, and 2-(2-butoxyethoxy)ethanol; glycol ethers such as ethylene glycol monomethyl ether and ethylene glycol monobutyl ether; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and diisobutyl ketone; and hydrocarbons such as toluene and xylene. One of these solvents may be used alone, or two or more may be used in combination.

[0043] The resin composition is thermosetting and may contain, for example, at least one selected from the group consisting of a compound having a cyanate group, a compound having a bismaleimide group, and a compound having an epoxy group, and a curing agent.

[0044] Examples of compounds having a cyanate group include dimethylmethylenebis(1,4-phenylene)biscyanate and bis(4-cyanatephenyl)methane. Dimethylmethylenebis(1,4-phenylene)biscyanate is commercially available, for example, as TACN (trade name, manufactured by Mitsubishi Gas Chemical Company, Inc.).

[0045] Examples of compounds having a bismaleimide group include N,N'-[(1-methylethylidene)bis[(p-phenylene)oxy(p-phenylene)]]bismaleimide and 4,4'-diphenylmethane bismaleimide. N,N'-[(1-methylethylidene)bis[(p-phenylene)oxy(p-phenylene)]]bismaleimide is commercially available, for example, as BMI-80 (trade name, manufactured by K.I. Chemical Co., Ltd.).

[0046] Examples of the compound having an epoxy group include bisphenol F epoxy resins, bisphenol A epoxy resins, biphenyl epoxy resins, and polyfunctional epoxy resins. For example, 1,6-bis(2,3-epoxypropan-1-yloxy)naphthalene, which is commercially available as HP-4032D (manufactured by DIC Corporation, trade name), may be used.

[0047] The curing agent may contain a phosphine-based curing agent and an imidazole-based curing agent. The phosphine-based curing agent can promote the triazine-producing reaction by trimerization of a compound having a cyanate group or a cyanate resin. Examples of phosphine-based curing agents include tetraphenylphosphonium tetra-p-tolylborate and tetraphenylphosphonium tetraphenylborate. Tetraphenylphosphonium tetra-p-tolylborate is commercially available, for example, as TPP-MK (trade name, manufactured by Hokko Chemical Industry Co., Ltd.).

[0048] Imidazole curing agents produce oxazoline and promote the curing reaction of compounds having epoxy groups or epoxy resins. Examples of imidazole curing agents include 1-(1-cyanomethyl)-2-ethyl-4-methyl-1H-imidazole and 2-ethyl-4-methylimidazole. 1-(1-cyanomethyl)-2-ethyl-4-methyl-1H-imidazole is commercially available, for example, as 2E4MZ-CN (trade name, manufactured by Shikoku Chemicals Corporation).

[0049] The resin composition may contain components other than the base resin and the curing agent, such as other resins such as phenolic resins, melamine resins, urea resins, and alkyd resins, silane coupling agents, leveling agents, antifoaming agents, surface conditioners, and wetting and dispersing agents.

[0050] The curing step may be carried out after the impregnation step, or may be carried out simultaneously with the impregnation step. In the curing step, the resin composition contained in the resin-impregnated body is cured to form filled and unfilled portions in the boron nitride sintered body. In the curing step, the resin composition is cured by heating and / or light irradiation, depending on the type of resin composition (or the type of curing agent added as needed). If the curing step is carried out immediately after the resin composition begins to impregnate the boron nitride sintered body, it is possible to stop the impregnation of the resin composition into the interior of the boron nitride sintered body.

[0051] In the curing step, the heating temperature when the resin composition is cured by heating may be, for example, 80 to 130°C. The resin obtained by curing the resin composition may contain, as resin components, at least one thermosetting resin selected from the group consisting of cyanate resins, bismaleimide resins, and epoxy resins, and a curing agent. In addition to these components, the resin may contain components derived from other resins such as phenolic resins, melamine resins, urea resins, and alkyd resins, as well as silane coupling agents, leveling agents, antifoaming agents, surface conditioners, and wetting and dispersing agents.

[0052] In this way, a composite can be obtained that includes a boron nitride sintered body having filled portions where the pores are filled with resin and unfilled portions where the pores are not filled with resin and are surrounded by the filled portions. The formation of the filled portions and unfilled portions in the boron nitride sintered body can be confirmed by observing the cross section of the composite with the naked eye or a microscope.

[0053] A coating process may be performed after the curing process to provide a resin layer covering the surface of the filled portion. In the coating process, a resin composition is attached to at least a portion of the surface of the filled portion formed in the curing process, and the resin is heated to coat at least a portion of the surface of the filled portion with the resin. Since the resin contained in the filled portion is cured, the filled portion prevents the resin composition from penetrating into the interior from its surface. The coating method is not particularly limited, and the composite (resin-filled body) obtained in the curing process may be immersed in the resin composition, or the resin composition may be applied to part or all of the surface of the composite. Depending on the type of resin composition (or a curing agent added as needed), the resin composition is cured by heating and / or light irradiation. If the resin in the filled portion is a thermosetting resin, dissolution of the resin in the filled portion can be prevented even when heated. In this way, a resin layer covering the surface of the filled portion can be formed.

[0054] The resin composition (second resin composition) used in the coating step may be the same as or different from the resin composition (first resin composition) used in the impregnation step. The components and curing rate of the resin layer provided on the surface of the filling portion in the coating step may be the same as or different from the resin filled in the pores of the filling portion. By the above steps, for example, a composite 100 as shown in FIG. 1 can be produced. However, the method for producing the composite 100 is not limited to the above production method.

[0055] In a variation of the above manufacturing method, the composite 100 may be obtained by adhering a sheet-shaped cured resin to the surface of the filling portion. In this variation, the use of a sheet-shaped cured resin allows for smooth production of a composite with excellent dimensional accuracy. Furthermore, the number of heating cycles can be reduced, allowing for efficient production of the composite. In another variation, the covering step may be omitted, and a composite without a resin layer formed of resin on the surface may be obtained by the curing step. In yet another variation, an excess of the resin composition may be attached to the surface of the resin-impregnated body before the curing step (for example, during the impregnation step), and the composite 100 whose surface is covered with a resin layer may be obtained by the curing step.

[0056] Although several embodiments have been described above, the present disclosure is not limited to the above embodiments. For example, in the sintering step, a boron nitride sintered body may be obtained by hot pressing, which simultaneously performs molding and sintering. Furthermore, the resin layer may be formed in an island shape rather than a layer shape. The shape of the composite is not limited to a block shape, but may also be cylindrical or spherical.

[0057] The present disclosure will be described in more detail with reference to examples and comparative examples, but the present disclosure is not limited to the following examples.

[0058] Example 1 Preparation of Boron Nitride Sintered Body Amorphous boron nitride powder (manufactured by Denka Company Limited, total oxygen content: 1.5 mass%, boron nitride purity: 97.0 mass%) and hexagonal boron nitride powder (manufactured by Denka Company Limited, total oxygen content: 0.3 mass%, boron nitride purity: 99.0 mass%, average particle size: 15 μm) were placed in a container in a weight ratio of 40:60. An organic binder and water were added to the container and mixed, followed by dry granulation to obtain a mixed powder.

[0059] The obtained mixed powder was filled into a cold isostatic pressing apparatus (CIP, manufactured by Kobe Steel, Ltd., product name: ADW800), and compressed under a pressure of 10 MPa to produce a compact (CIP molding pressure: 10 MPa).

[0060] In order to decompose and remove the organic binder, the produced compact was heat treated at a heating temperature of 600° C. for 5 hours, and the organic binder component was decomposed and removed from the compact to obtain a degreased body.

[0061] The degreased body was introduced into a batch-type high-frequency furnace (manufactured by Fuji Radio Industrial Co., Ltd.) and subjected to a first firing at 1400°C for 2 hours, followed by a second firing at 2050°C for 10 hours, to obtain a boron nitride sintered body having a rectangular prism shape. During firing, nitrogen gas was circulated through the furnace at a flow rate of 10 L / min under standard conditions. In this way, firing was carried out under a nitrogen atmosphere at a pressure of 0.1 MPa (atmospheric pressure).

[0062] [Evaluation of Boron Nitride Sintered Body] <Measurement of Thickness, Bulk Density, and Porosity> The size and weight of the obtained boron nitride sintered body were measured, and the bulk density (g / cm 3 The size of the boron nitride sintered body was length x width x thickness = 45 mm x 50 mm x 35 mm. The bulk density of the boron nitride sintered body was determined in accordance with JIS Z 8807:2012 "Method for measuring density and specific gravity by geometric measurement," based on the volume calculated from the length of each side of the boron nitride sintered body (measured with a vernier caliper) and the weight of the boron nitride sintered body measured with an electronic balance (see Section 9 of JIS Z 8807:2012). The bulk density and the theoretical density of boron nitride (2.26 g / cm 3 ), the porosity was calculated by the following calculation formula (1): In calculation formula (1), B is the bulk density (g / cm 3 The thickness, bulk density, and porosity were as shown in Table 1. Porosity (volume %) = [1 - (B / 2.26)] x 100 (1)

[0063] <Measurement of average pore diameter> The pore volume distribution of the boron nitride sintered body was measured using a mercury porosimeter (device name: Autopore IV9500) manufactured by Shimadzu Corporation. The measurement was carried out while increasing the pressure from 0.0042 MPa to 206.8 MPa. The pore diameter at which the cumulative pore volume reached 50% of the total pore volume was defined as the "average pore diameter." The results are shown in Table 1.

[0064] [Preparation of Resin-Impregnated Body] As shown in Figure 3, a black stripe-shaped line 30 was drawn on the surface of the boron nitride sintered body 11 using a black oil paint. This makes it easier to see the boundary between the resin-impregnated and non-impregnated areas in the final composite. A resin composition was prepared by blending 10 parts by weight of a commercially available curing agent (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., product name: Acmex H-8) with 100 parts by weight of a commercially available epoxy resin (manufactured by Mitsubishi Chemical Corporation, product name: Epicoat 807). The prepared resin composition was heated at 120°C for 15 minutes.

[0065] This resin composition was degassed for 10 minutes under a vacuum of 100 Pa, and then poured into a container containing the boron nitride sintered body under vacuum, and allowed to soak for 20 minutes.

[0066] [Preparation of Composite] The resin-impregnated body was heated at 160° C. for 60 minutes under atmospheric pressure to cure the resin composition, thereby obtaining a composite containing the boron nitride sintered body and the resin filling the pores thereof.

[0067] [Evaluation of the composite] The shape and size of the composite were almost the same as those of the boron nitride sintered body. The weight of the composite was measured, and the difference between the weight of the composite and the weight of the boron nitride sintered body was taken as the weight of the resin. The ratio of the weight of the resin to the total weight of the composite was calculated. The results are shown in the "Weight ratio of resin" column in Table 1.

[0068] The composite was cut parallel to a pair of surfaces facing each other in the thickness direction and through the center of the composite. The cross section thus obtained was visually observed. This cross section corresponds to the cross section along line IV-IV in Figure 3 and was obtained by cutting along the portion indicated by the black strip line 30. Cross-sectional observation confirmed that resin was not present in the central portion, including the center, and that resin was present only in the surface portion. In other words, an unfilled portion was formed inside the boron nitride sintered body, with a filled portion formed around it. A boron nitride sintered body with an unfilled portion formed in this manner was evaluated as having an unfilled portion. The cross-sectional area W of the entire cross section of the boron nitride sintered body and the cross-sectional area N of the unfilled portion in the cross section were measured. The ratio (N / W) of the cross-sectional area N of the unfilled portion to the cross-sectional area W of the entire cross section was as shown in Table 1.

[0069] Example 2 A boron nitride sintered body and a composite were produced and evaluated in the same manner as in Example 1, except that the CIP molding pressure when producing the compact was set to 20 MPa. The evaluation results are shown in Table 1.

[0070] Example 3 A boron nitride sintered body and a composite were produced and evaluated in the same manner as in Example 1, except that the CIP molding pressure when producing the compact was set to 40 MPa. The evaluation results are shown in Table 1.

[0071] Example 4 A boron nitride sintered body and a composite were produced and evaluated in the same manner as in Example 1, except that the CIP molding pressure when producing the compact was 100 MPa. The evaluation results are shown in Table 1.

[0072] Example 5 A boron nitride sintered body and a composite were produced and evaluated in the same manner as in Example 1, except that the CIP molding pressure when producing the compact was set to 500 MPa. The evaluation results are shown in Table 1.

[0073] Example 6 A boron nitride sintered body and a composite body were produced and evaluated in the same manner as in Example 1, except that the amount of raw material powder was increased to obtain a boron nitride sintered body with a thickness of 100 mm. The evaluation results are shown in Table 1.

[0074] Comparative Example 1 A boron nitride sintered body and a composite were produced and evaluated in the same manner as in Example 1, except that the CIP molding pressure when producing the compact was set to 5 MPa. The evaluation results are shown in Table 1.

[0075]

[0076] FIG. 4(A) is a cross-sectional photograph of the composite of Example 3. As shown in FIG. 4(A), the composites of each Example had unfilled portions 12 that were not filled with resin, surrounded by filled portions 14 that were filled with resin. The composites also had a resin layer 20 made of resin that covered the filled portions 14. The boundary 13 between the filled portions 14 and the unfilled portions 12 had a shape similar to the outer edge of the composite. As shown in FIG. 4(B), the composite of Comparative Example 1 had resin filled throughout the boron nitride sintered body, and there were no unfilled portions 12. Due to the position where the black paint was applied, four white areas were present in a lattice pattern inside, and these areas were also filled with resin.

[0077] 10, 10A, 11...boron nitride sintered body, 12...unfilled portion, 13...boundary, 14...filled portion, 14e...edge, 20...resin layer, 30...strip-shaped black line, 100, 100A...composite

Claims

1. A composite comprising a porous boron nitride sintered body and a resin filled into some of the pores of the boron nitride sintered body, wherein the boron nitride sintered body has a filled portion in which the pores are filled with the resin, and an unfilled portion surrounded by the filled portion in which the pores are not filled with the resin.

2. The composite according to claim 1, further comprising a resin layer covering at least a portion of said filling portion.

3. The composite according to claim 1 or 2, wherein the porosity of the boron nitride sintered body is 56 volume % or less.

4. The composite according to claim 1 or 2, wherein the average pore size of the pores in the boron nitride sintered body is 1.5 μm or less.

5. The composite according to claim 1 or 2, wherein the filling portion in the boron nitride sintered body has an edge protruding outward.

6. The composite according to claim 1 or 2, wherein the thickness of the boron nitride sintered body is 30 mm or more.

7. The composite according to claim 1 or 2, wherein the ratio of a cross-sectional area N of said unfilled portion to a cross-sectional area W of said boron nitride sintered body is 0.2 or more.

8. The composite according to claim 1 or 2, wherein the volume of the non-filled portion is greater than the volume of the filled portion.

9. A method for producing a composite, comprising: an impregnation step of impregnating pores in the surface portion of a porous boron nitride sintered body with a resin composition to obtain a resin-impregnated body; and a curing step of heating the resin-impregnated body to harden the resin composition and form a filled portion, in which the pores are filled with resin, and an unfilled portion, surrounded by the filled portion, in which the pores are not filled with resin.

10. The method for producing a composite body according to claim 9, wherein the porosity of the boron nitride sintered body is 56 volume % or less, and the average pore size of the pores is 1.5 μm or less.

Citation Information

Patent Citations

  • Heat radiation member and its use

    JP2015096456A

  • Resin-impregnated boron nitride sintered body and use for same

    WO2014196496A1

  • Method for producing composite body

    WO2020203688A1

  • Composite body and method for manufacturing same, and laminated body and method for manufacturing same

    WO2022209971A1

Cited By

  • Resin-filled boron nitride sintered structures and electronic devices containing the same, and methods for manufacturing the same.

    JP7942476B1

  • Silicone resin composition

    WO2025249161A1