Foamed polylactic acid resin sheet and method for producing formed sheet

The use of a polylactic acid resin foam sheet with controlled crystallinity and a two-stage heating process addresses the heat resistance and efficiency challenges in producing sheet molded products, resulting in improved thermal performance and production efficiency.

WO2024204489A1PCT designated stage expired Publication Date: 2024-10-03SEKISUI PLASTICS CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012549
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional polylactic acid resin foam sheets made from amorphous materials lack sufficient heat resistance, which hinders their use in sheet molded products, and crystalline forms require lengthy heat setting processes, reducing production efficiency.

Method used

A polylactic acid resin foam sheet with crystallinity of 30% or less, produced using a method involving primary and secondary heating steps to increase crystallinity, is used for thermoforming, optimizing heat resistance and manufacturing efficiency.

Benefits of technology

The method enables the production of sheet molded bodies with enhanced heat resistance and improved manufacturing efficiency by controlling crystallinity and heat treatment processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012549_03102024_PF_FP_ABST
    Figure JP2024012549_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a foamed polylactic acid resin sheet suitable for efficiently producing a formed sheet having excellent heat resistance, and improves the efficiency of producing a formed sheet having excellent heat resistance. The foamed polylactic acid resin sheet is constituted from a polylactic acid resin composition containing a polylactic acid resin having crystallinity, and has a degree of crystallinity of 30% or less and a crystallization temperature, as observed by heat-flux differential scanning calorimetry at a heating rate of 5°C / min, of 105°C or lower.
Need to check novelty before this filing date? Find Prior Art

Description

Polylactic acid resin foam sheet and method for manufacturing sheet molded body CROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This application claims priority from Japanese Patent Application No. 2023-052796, the disclosure of which is incorporated herein by reference.

[0002] The present invention relates to a polylactic acid resin foam sheet and a method for producing a sheet molded article using the polylactic acid resin foam sheet.

[0003] Foamed products made of foamed resin compositions have been widely used. These foamed products are lightweight yet strong, and offer excellent cushioning and heat insulation properties. Known examples of this type of foamed product include foamed sheets and foamed beads, as well as molded articles made from these. A known example of a resin foam sheet is an extruded foam sheet obtained by melt-kneading a foaming resin composition and a foaming agent in an extruder, and then extruding the resulting molten mixture into a sheet through a sheeting die (a flat die or a circular die) attached to the tip of the extruder, thereby foaming the extruded foam.

[0004] This type of extruded foam sheet is used as a cushioning sheet in its sheet form, or formed into a bag shape and used as a packaging material. This type of extruded foam sheet is also widely used as a base sheet for sheet molded articles such as food trays and cups. This type of sheet molded article is produced by thermoforming such as match mold forming or vacuum / pressure forming.

[0005] Recently, there has been a growing demand for measures to address the problem of landscape damage caused by illegally dumped packaging materials in places such as mountains, fields, rivers, and coastlines. Against this background, the production of molded articles using polylactic acid resins that can be biodegraded in the natural environment has been studied, and the use of polylactic acid resin foam sheets in various applications has been investigated.

[0006] Many conventional polylactic acid resin foam sheets are made from amorphous polylactic acid resin, which is easily foamed. However, such polylactic acid resin foam sheets and sheet molded articles made from such polylactic acid resin foam sheets often lack sufficient heat resistance. For this reason, the use of crystalline polylactic acid resins is increasing. Accordingly, there are also increasing opportunities to produce polylactic acid resin foam sheets from resin compositions containing crystalline polylactic acid resins. Such polylactic acid resin foam sheets are easier to thermoform if they are not crystallized. Therefore, when producing sheet molded articles from polylactic acid resin foam sheets made from crystalline polylactic acid resins, polylactic acid resin foam sheets manufactured in a state where crystallization is suppressed are used. During thermoforming, the polylactic acid resin foam sheet is heated for a certain period of time to increase the crystallinity (see, for example, paragraphs 0059-0061 of Patent Document 1 below).

[0007] Japanese Patent No. 5517280

[0008] When producing a sheet molded body using a polylactic acid resin foam sheet containing a crystalline polylactic acid resin, a step called "heat setting" is performed during thermoforming, in which the sheet is held in a heated mold for a certain period of time to increase the crystallinity. If a polylactic acid resin foam sheet with a sufficiently low crystallinity is used to ensure moldability, the heat setting process takes a long time, reducing the production efficiency of the sheet molded body. In view of the above problems, the present invention aims to provide a polylactic acid resin foam sheet suitable for efficiently producing a sheet molded body with excellent heat resistance, thereby improving the production efficiency of the sheet molded body with excellent heat resistance.

[0009] In order to solve the above problems, the present invention provides a polylactic acid resin foam sheet composed of a polylactic acid resin composition containing a crystalline polylactic acid resin, wherein the polylactic acid resin foam sheet has a crystallinity of 30% or less and a crystallization temperature of 105°C or less as observed by heat flux differential scanning calorimetry at a heating rate of 5°C / min.

[0010] In order to solve the above-mentioned problems, the present invention provides a method for producing a sheet molded body by thermoforming a resin foam sheet, wherein the resin foam sheet is a polylactic acid resin foam sheet made of a polylactic acid resin composition containing a crystalline polylactic acid resin, the resin foam sheet having a crystallinity of 30% or less and a crystallization temperature of 105°C or less as observed by heat flux differential scanning calorimetry at a heating rate of 5°C / min, the method comprising the steps of: a primary heating step of heating the polylactic acid resin foam sheet; and a secondary heating step of sandwiching the polylactic acid resin foam sheet that has been subjected to the primary heating step between heated molds to produce a sheet molded body and increase the crystallinity of the sheet molded body.

[0011] Fig. 1 is a schematic front view showing an example of a sheet manufacturing apparatus for manufacturing a polylactic acid resin foam sheet. Fig. 2 is a schematic view showing a method for determining the half-crystallization time from a DSC curve. Fig. 3 is a schematic perspective view showing a method for measuring the gel fraction.

[0012] An embodiment of the present invention will be described below. Hereinafter, the embodiment of the present invention will be described taking as an example a case where the polylactic acid resin foam sheet is an extruded foam sheet obtained by an apparatus such as that shown in FIG. 1. The polylactic acid resin foam sheet of this embodiment can be suitably used to produce a sheet molded product by thermoforming. Examples of such thermoforming include vacuum forming, pressure forming, vacuum-pressure forming, matched mold forming, and press forming.

[0013] The polylactic acid resin foam sheet of this embodiment may be, for example, an extruded foam sheet produced by a sheet manufacturing apparatus 100 illustrated in Fig. 1. The sheet manufacturing apparatus 100 illustrated in Fig. 1 includes a tandem extruder 10 and a circular die CD that extrudes the polylactic acid resin composition melt-kneaded in the tandem extruder 10 into a cylindrical shape. The manufacturing apparatus further includes a cooling device CL that air-cools the polylactic acid resin foam sheet extruded into a cylindrical shape from the circular die CD, and a mandrel MD that expands the diameter of the cylindrical polylactic acid resin foam sheet to form a cylindrical shape of a predetermined size.

[0014] The sheet manufacturing apparatus 100 is equipped with a slitting device that slits the polylactic acid resin foam sheet after it has passed through the mandrel MD and become a cylindrical shape having a predetermined diameter, and divides it into two strip-shaped sheets, and a winding roller 22 that winds up the slit polylactic acid resin foam sheet 1 after passing it through multiple rollers 21.

[0015] The extruder upstream of the tandem extruder 10 (hereinafter also referred to as the "first extruder 10a") is provided with a hopper 11 for feeding a polylactic acid resin composition (hereinafter also simply referred to as the "resin composition"), which is the raw material for the polylactic acid resin foam sheet, and a gas inlet 12 for supplying a foaming agent such as a hydrocarbon into the cylinder.

[0016] The sheet manufacturing apparatus 100 of this embodiment is also provided with an extruder (hereinafter also referred to as the "second extruder 10b") downstream of the first extruder 10a. The second extruder 10b melt-mixes a resin composition containing a foaming agent. The polylactic acid resin contained in the polylactic acid resin foam sheet has crystalline properties. The polylactic acid resin is preferably modified by crosslinking or the like so as to exhibit excellent melt tension. The modified polylactic acid resin (hereinafter also referred to as the "modified polylactic acid resin") may be introduced from the hopper 11 after being previously modified. When producing a polylactic acid resin foam sheet, unmodified polylactic acid resin and a crosslinking agent may be introduced into the extruder, and the polylactic acid resin may be modified in the extruder.

[0017] Polylactic acid resin foam sheets crystallize if not cooled quickly. The polylactic acid resin foam sheet of this embodiment is produced so that the cooling device CL and mandrel MD prevent the crystallization of the contained polylactic acid resin during production. A polylactic acid resin foam sheet containing sufficiently crystallized polylactic acid resin is resistant to deformation even when heated. Such a polylactic acid resin foam sheet is less likely to deform to the shape of a mold during thermoforming. Furthermore, such a polylactic acid resin foam sheet is stretched with a strong force during thermoforming. The sheet molded product obtained in this manner tends to shrink over time or when heated. On the other hand, the polylactic acid resin foam sheet of this embodiment is produced to have a crystallinity of 30% or less. A polylactic acid resin foam sheet with a lower crystallinity has better moldability when producing a sheet molded product. Therefore, the crystallinity of the polylactic acid resin foam sheet may be 25% or less, or even 20% or less. By ensuring that the crystallinity is 30% or less, excessive stretching in the mold during thermoforming can be prevented, and shrinkage over time in the resulting sheet molded body can be prevented.

[0018] It is advantageous for the polylactic acid resin foam sheet to have a certain degree of crystallinity or higher in order to provide a sheet molding with sufficient crystallinity to exhibit excellent heat resistance. The crystallinity of the polylactic acid resin foam sheet may be 5% or higher, or 10% or higher.

[0019] It is preferable that the polylactic acid resin foam sheet exhibits a higher degree of crystallinity than before heating through a process such as heat setting in which the sheet is heated for a certain period of time. The polylactic acid resin foam sheet is preferably formed so as to increase the degree of crystallinity by 5% or more, and preferably so as to increase the degree of crystallinity by 10% or more. The degree of crystallinity that the polylactic acid resin foam sheet can achieve is preferably 25% or more, and more preferably 30% or more. The degree of crystallinity that the polylactic acid resin foam sheet can achieve is usually 60% or less. The degree of crystallinity that the polylactic acid resin foam sheet can achieve may be 50% or less.

[0020] The resin composition constituting the polylactic acid resin foam sheet of this embodiment preferably has a half-crystallization time of 30 minutes or less at 80°C. The half-crystallization time is more preferably 25 minutes or less. When the resin composition constituting the polylactic acid resin foam sheet has a half-crystallization time of 30 minutes or less, the crystallinity of the sheet molding can be increased in a shorter molding time during thermoforming, and excellent heat resistance can be imparted to the sheet molding.

[0021] (Crystallization Half Time) The crystallization half time can be measured using a heat flux differential scanning calorimeter (heat flux DSC) as follows. However, the sampling method and temperature conditions are as follows. 5.5±0.5 mg of a sample is packed into the bottom of an aluminum measurement container (Hitachi High-Tech Science Corporation, product code: GAA-0065) so that there are no gaps, and then an aluminum lid (Hitachi High-Tech Science Corporation, product code: GAA-0064) is placed on it. Next, using a differential scanning calorimeter (Hitachi High-Tech Science Corporation, "NEXTA DSC600"), the sample is held at 30°C for 2 minutes under a nitrogen gas flow rate of 20 mL / min, and then heated from 30°C to 210°C (first heating) at the maximum capacity rate of the device, and maintained there for 10 minutes. Thereafter, the sample is removed from the measurement device, allowed to stand at room temperature for 10 minutes, and then returned to the measurement device at 30°C. Second temperature increase: After increasing the temperature to 70°C at the maximum capacity of the device, increase the temperature to 80°C at a rate of 20°C / min and hold for 30 minutes. Alumina is used as the reference material.

[0022] (Method of Preparing a DSC Curve) From the start of the second heating to the end of the holding time at the heating end temperature, the heat flow was read every 0.2 seconds and plotted with time (min) on the horizontal axis and heat flow (mW) on the vertical axis to prepare a DSC curve (see Figure 2). In Figure 2, the time from the start of measurement to the peak top (point x) of the exothermic peak is defined as the half-crystallization time.

[0023] The resin composition contains a crystalline polylactic acid resin as a main component. The polylactic acid resin refers to a polymer containing 50 mol% or more of lactic acid component units. Examples of such polymers include: (1) polymers of lactic acid alone; (2) copolymers of lactic acid and other aliphatic hydroxycarboxylic acids; (3) copolymers of lactic acid, aliphatic polyhydric alcohols, and aliphatic polycarboxylic acids; (4) copolymers of lactic acid and aliphatic polycarboxylic acids; (5) copolymers of lactic acid and aliphatic polyhydric alcohols; and (6) mixtures of any of the above (1) to (5).

[0024] Specific examples of the lactic acid include L-lactic acid, D-lactic acid, DL-lactic acid, or their cyclic dimers, L-lactide, D-lactide, DL-lactide, or mixtures thereof.

[0025] Examples of the aliphatic polycarboxylic acid constituting the copolymer include oxalic acid, succinic acid, malonic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, undecanedioic acid, and dodecanedioic acid. The aliphatic polycarboxylic acid may be an anhydride.

[0026] Examples of the aliphatic polyhydric alcohol include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, 1,3-butanediol, 1,4-butanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,9-nonanediol, neopentyl glycol, tetramethylene glycol, and 1,4-cyclohexanedimethanol.

[0027] Examples of the aliphatic hydroxycarboxylic acid other than lactic acid that constitutes the copolymer include glycolic acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 4-hydroxyvaleric acid, 5-hydroxyvaleric acid, and 6-hydroxycaproic acid.

[0028] The polylactic acid resin contained in the resin composition may be a crystalline polylactic acid resin alone, or may contain a crystalline polylactic acid resin and an amorphous polylactic acid resin.

[0029] The polylactic acid resin may have an endothermic capacity (ΔHendo) of, for example, 10 J / g or more as determined by heat flux differential scanning calorimetry. The endothermic capacity (ΔHendo) of the polylactic acid resin is preferably 20 J / g or more, and more preferably 30 J / g or more. The upper limit of the endothermic capacity (ΔHendo) of the polylactic acid resin is not particularly limited, but is generally 60 J / g.

[0030] In this embodiment, the crystalline polylactic acid resin refers to one having an endothermic heat (ΔHendo) of more than 2 J / g as determined by heat flux differential scanning calorimetry. The endothermic heat (ΔHendo) of the crystalline polylactic acid is usually 20 to 65 J / g.

[0031] The polylactic acid resin contained in the resin composition preferably contains a copolymer in which the D- and L-forms of lactic acid are copolymerized. The proportion of the D-form in the copolymer is preferably 0.5 mol % or more and 5 mol % or less. The polylactic acid resin containing the copolymer preferably has a melting point of 130°C or more and 170°C or less. Such a polylactic acid resin has excellent properties in terms of foamability, moldability, and heat resistance.

[0032] The polylactic acid resin foam sheet of this embodiment preferably has a crystallization temperature of 105°C or lower as confirmed by heat flux differential scanning calorimetry at a heating rate of 5°C / min. The crystallization temperature of the polylactic acid resin foam sheet is more preferably 100°C or lower, and even more preferably 98°C or lower. Having a crystallization temperature below a predetermined temperature allows the polylactic acid resin foam sheet to rapidly crystallize during thermoforming. Such a polylactic acid resin foam sheet has excellent moldability. Furthermore, to prevent an excessive increase in crystallinity during preheating before thermoforming, the crystallization temperature is preferably in the range of 70°C or higher, more preferably 75°C or higher, and even more preferably 80°C or higher.

[0033] (Melting Point, Crystallization Temperature, Crystallinity) The melting point, crystallization temperature, and crystallinity of polylactic acid resin, polylactic acid resin foam sheet, and sheet molded article can be determined as follows. The melting point and crystallization temperature of polylactic acid resin, polylactic acid resin foam sheet, and sheet molded article can be measured as follows using a heat flux differential scanning calorimeter (heat flux DSC). The measurement is carried out according to the methods described in JIS K7122:1987, JIS K7122:2012 "Method for measuring the heat of transition of plastics" and JIS K7121:1987, 2012 "Method for measuring the transition temperature of plastics." The sampling method and temperature conditions can be as follows. A sample was packed to the bottom of an aluminum measurement container (Hitachi High-Tech Science Corporation, product code: GAA-0065) with 5.5±0.5 mg of sample, leaving no gaps. An aluminum lid (Hitachi High-Tech Science Corporation, product code: GAA-0064) was then placed on the container. A DSC curve was then obtained using a differential scanning calorimeter (Hitachi High-Tech Science Corporation, "NEXTA DSC600") under a nitrogen gas flow rate of 20 mL / min, by heating and cooling the sample in the following steps: (Step 1) The sample was heated from 30°C to 210°C (first heating), and then held for 10 minutes. (Step 2) The sample was removed from the measurement device, allowed to stand at room temperature for 10 minutes, and then returned to the measurement device at 30°C (rapid cooling). (Step 3) The sample was heated from 30°C to 210°C (second heating). All heating was performed at a rate of 5°C / min. Alumina is used as the reference material.

[0034] (Melting Point) Using the analysis software provided with the apparatus, the temperature at the top of the melting peak observed during the second heating process is read and used as the melting temperature (melting point). (Crystallization Temperature) The crystallization temperature is the (cold) crystallization temperature, which is read as the temperature at the top of the exothermic peak observed during the second heating process. If multiple exothermic peaks appear, the temperature of the lower temperature peak is read. (Crystallization Degree) The crystallization degree is determined by dividing the difference between the endothermic amount (heat of fusion (J / g)) calculated from the area of ​​the endothermic peak appearing in the crystalline melting observed during the first heating process and the heat of crystallization (J / g) calculated from the area of ​​the crystallization peak, by the theoretical heat of fusion of perfectly crystalline polylactic acid (93 J / g). The heat of fusion and heat of crystallization are calculated using the analysis software provided with the apparatus. Specifically, the heat of fusion is calculated from the area enclosed by the line connecting the point where the DSC curve departs from the low-temperature baseline and the point where the DSC curve returns to the high-temperature baseline, and the DSC curve. The heat of crystallization is calculated from the area enclosed by the line connecting the point where the DSC curve departs from the low-temperature baseline and the point where the DSC curve returns to the high-temperature baseline, and the DSC curve. The degree of crystallization is calculated from the following formula: Degree of crystallization (%) = [heat of fusion (J / g) - heat of crystallization (J / g)] / 93 (J / g) × 100 (%)

[0035] The resin composition may contain the polylactic acid resin in a proportion of 100% by mass, or may be a mixture of the polylactic acid resin and a thermoplastic resin other than the polylactic acid resin. The mixture may contain the polylactic acid resin in a proportion of 50% by mass or more but less than 100% by mass, and the thermoplastic resin in a proportion of more than 0% by mass but not more than 50% by mass. That is, the resin composition may contain the thermoplastic resin other than the polylactic acid resin in a proportion of 50% by mass or less.

[0036] When the resin composition contains a thermoplastic resin other than the polylactic acid resin, the proportion of the polylactic acid resin is preferably 60% by mass or more, more preferably 70% by mass or more. Examples of thermoplastic resins other than the polylactic acid resin include polyethylene-based resins, polypropylene-based resins, polystyrene-based resins, and polyester-based resins. In this embodiment, the resin composition preferably contains a thermoplastic elastomer or an aliphatic polyester resin, from the viewpoint of improving the impact resistance of a sheet molding made from a polylactic acid resin foam sheet.

[0037] Examples of the thermoplastic elastomer include olefin-based elastomers, styrene-based elastomers, acrylic elastomers, and ester-based elastomers. Among these, acrylic elastomers, styrene-based elastomers, and ester-based elastomers are preferred because they have good compatibility with polylactic acid resins. It is preferable that the styrene-based elastomers are acid-modified. Specifically, commercially available products such as Metablen W-600A manufactured by Mitsubishi Rayon Co., Ltd., Tuftec MP10 manufactured by Asahi Kasei Corporation, and Nofalloy TZ810 manufactured by NOF Corporation can be suitably used.

[0038] The aliphatic polyester resin may be a hydroxy acid polycondensate, a ring-opening polymerization product of lactone, or a polycondensate of a polyhydric alcohol component and a polycarboxylic acid component. Examples of hydroxy acid polycondensates include polylactic acid and polycondensates of hydroxybutyric acid. Examples of ring-opening polymerization products of lactone include polycaprolactone and polypropiolactone. Examples of polycondensates of a polyhydric alcohol component and a polycarboxylic acid component include polyethylene succinate, polybutylene succinate, polybutylene adipate, polybutylene succinate adipate, and polybutylene adipate terephthalate. Among these, the aliphatic polyester resin is preferably polybutylene succinate (PBS), polybutylene succinate adipate (PBSA), or polybutylene adipate terephthalate (PBAT), which have good compatibility with polylactic acid resins.

[0039] The polylactic acid resin is preferably suitable for extrusion foaming. It is known that in extrusion foaming, a foamed sheet with a high expansion ratio can generally be obtained by using a resin with a high melt tension. Crystalline resins generally have a low melt tension. Therefore, when extrusion foaming a crystalline resin, the crystalline resin is subjected to crosslinking such as chemical crosslinking or electron beam crosslinking in order to increase the melt tension of the resin composition. Furthermore, instead of crosslinking the crystalline resin, a method of increasing the melt tension of the resin composition by mixing a high molecular weight component is known.

[0040] The polylactic acid resin of this embodiment preferably exhibits a specific characteristic value in melt tension measurement at 190°C. For example, the polylactic acid resin preferably exhibits a melt tension of 5 cN or more and 80 cN or less in measurement at 190°C. The melt tension of the polylactic acid resin may be 75 cN or less, 70 cN or less, or 65 cN or less. The melt tension of the polylactic acid resin may be 8 cN or more, or 10 cN or more. By having the above-described preferable melt tension, the polylactic acid resin can suppress cell breakage during foaming of the resin composition. A polylactic acid resin foam sheet containing such a polylactic acid resin is unlikely to have a high open cell ratio even when foamed at a high expansion ratio. Such a polylactic acid resin can be advantageous for producing a polylactic acid resin foam sheet with good appearance.

[0041] In this embodiment, it is preferable that the resin composition containing the polylactic acid resin as described above also exhibits the melt tension as described above.

[0042] The polylactic acid resin of this embodiment has a melt mass-flow rate (MFR: temperature 190°C, nominal load 2.16 kg) of, for example, 0.1 g / 10 min or more and 15 g / 10 min or less. The melt mass-flow rate of the resin composition may be 10 g / 10 min or less, 5 g / 10 min or less, 4 g / 10 min or less, or 3 g / 10 min or less.

[0043] In this embodiment, it is preferable that the resin composition containing the polylactic acid resin as described above also exhibits the melt mass flow rate as described above.

[0044] The melt tension and melt mass-flow rate of the polylactic acid resin can be measured by the following method.

[0045] <Melt Tension> Melt tension can be measured using a Toyo Seiki Seisakusho "Capillograph 1D" (special furnace specification) capillary rheometer and a Goettfert "Rheotens 71.97." Melt tension measurements are performed under the following conditions. The sample is vacuum-dried at 90°C for at least 4 hours. After drying, it is placed in a nylon plastic bag for vacuum packing, vacuum-packed, and stored in a desiccator until immediately before measurement. The Rheotens 71.97 is installed so that the distance from the die exit of the Capillograph 1D to the measurement section is 80 mm. (Note: If interference prevents the Rheotens from being able to approach 80 mm, measures to avoid interference should be taken to set the Rheotens in the designated location.) First, the sample is filled into a barrel heated to a test temperature of 190°C and preheated for 5 minutes. The measurement time, including the preheating time after filling the barrel, should not exceed 10 minutes. Next, a piston is inserted from the top of the barrel and the molten resin is extruded into a string. At this time, the piston descending speed (20 mm / min) is kept constant and the extruded string-like material is passed through a Rheotens wheel. Thereafter, the take-up speed is gradually increased and the melt tension of the sample is measured. Regarding the measurement results, the average of the maximum and minimum tension values ​​just before the point at which the string-like material breaks is taken as the melt tension of the sample. Note that if there is only one maximum point on the tension chart, that maximum value is taken as the melt tension. Furthermore, if the string-like material becomes thinner and the winding becomes idle, that point is considered to be the break point, and the average of the maximum and minimum tension values ​​just before that point is taken as the melt tension of the sample.

[0046] (Measurement conditions for Capillograph 1D) Die: diameter 2.095 mm, length 8 mm, inlet angle 90 degrees (conical) Barrel diameter: 9.55 mm Piston speed: 20 mm / min Measurement temperature: 190°C

[0047] (Rheotensile measurement conditions) Wheel spacing: upper 0.7 mm, lower 1.0 mm Acceleration: 10 mm / s 2 Pull-up speed: Initial speed 6.92 mm / s

[0048] <Melt Mass-Flow Rate (MFR)> The melt mass-flow rate (MFR) of polylactic acid resins and resin compositions can be measured using a "Semi-Auto Melt Indexer 2A" manufactured by Toyo Seiki Seisakusho, Ltd. MFR is measured in accordance with the method of measuring the time it takes for a piston to move a predetermined distance described in JIS K7210-1:2014 "Plastics - Determination of Melt Mass-Flow Rate (MFR) and Melt Volume-Flow Rate (MVR) of Thermoplastic Plastics - Part 1," Method B, under the following measurement conditions. The measurement sample is vacuum-dried at 90°C for at least 4 hours, and after drying, it is placed in a nylon plastic bag for vacuum packing, vacuum-packed, and stored in a desiccator until immediately before measurement.

[0049] (Measurement conditions) Sample: 3 to 8 g Preheating time: 200 seconds Load hold: 30 seconds Test temperature: 190°C Test load: 21.18 N Piston movement distance (interval): 4 mm Number of tests: 3 The arithmetic mean of the measured values ​​obtained in each test is taken as the MFR (g / 10 min) value.

[0050] The above-mentioned thermal melting properties can be exhibited by imparting a bulky molecular structure to the polylactic acid resin. The polylactic acid resin preferably has a mass average molecular weight (Mw) of 100,000 or more and 1,000,000 or less. The mass average molecular weight (Mw) of the polylactic acid resin is more preferably 150,000 or more, and even more preferably 200,000 or more. The mass average molecular weight (Mw) of the polylactic acid resin is more preferably 800,000 or less, even more preferably 600,000 or less, and particularly preferably 400,000 or less.

[0051] The polylactic acid resin of this embodiment preferably has a ratio (Mw / Mn) of the mass average molecular weight (Mw) to the number average molecular weight (Mn) of 2.5 or more, more preferably 2.7 or more, and particularly preferably 2.9 or more. The ratio (Mw / Mn) of the polylactic acid resin is preferably 4.5 or less, more preferably 4.0 or less, and particularly preferably 3.5 or less.

[0052] The number average molecular weight (Mn) and mass average molecular weight (Mw) of the polylactic acid resin can be measured using gel permeation chromatography (GPC) and can be calculated as a polystyrene (PS) equivalent value. Specifically, the average molecular weight of the polylactic acid resin can be calculated by the following procedure.

[0053] (Method of determining average molecular weight) 20 mg of a sample was dissolved in 6 mL of chloroform (immersion time: 6±1.0 h), filtered through a non-aqueous 0.45 μm syringe filter manufactured by Shimadzu GLC Corporation, and then measured using a chromatograph under the following measurement conditions, and the mass average molecular weight of the sample was determined from a standard polystyrene calibration curve prepared in advance.

[0054] <Apparatus used> Tosoh Corporation "HLC-8320GPC EcoSEC" gel permeation chromatograph (built-in RI detector and UV detector) <GPC measurement conditions> Sample side: Guard column = Tosoh Corporation TSK guard column HXL-H (6.0 mm x 4.0 cm) x 1 Measurement column = Tosoh Corporation TSKgel GMHXL (7.8 mm I.D. x 30 cm) x 2 in series Reference side: Restrictor tube (inner diameter 0.1 mm x 2 m) x 2 in series Column temperature = 40°C Mobile phase = chloroform Mobile phase flow rate: Reference side pump = 0.5 mL / min Sample side pump = 1.0 mL / min Detector = RI detector Injection volume = 50 μL Measurement time = 25 min Sampling pitch = 500 msec

[0055] The standard polystyrene samples for the calibration curve are "STANDARD SM-105" and "STANDARD SH-75" manufactured by Showa Denko K.K., and have mass average molecular weights of 5,620,000, 3,120,000, 1,250,000, 442,000, 151,000, 53,500, 17,000, 7,660, 2,900, and 1,320. The polystyrene standards for the calibration curve were grouped into groups A (5,620,000, 1,250,000, 151,000, 17,000, 2,900) and B (3,120,000, 442,000, 53,500, 7,660, 1,320), and then 2 mg, 3 mg, 4 mg, 4 mg, and 4 mg of A were weighed and dissolved in 30 mL of chloroform. Similarly, 3 mg, 4 mg, 4 mg, 4 mg, and 4 mg of B were weighed and dissolved in 30 mL of chloroform. The standard polystyrene calibration curve was obtained by injecting 50 μL of each of the prepared solutions A and B and creating a calibration curve (cubic equation) from the retention times obtained after measurement. The average molecular weight was calculated using the calibration curve.

[0056] Polylactic acid resins with such melting properties and molecular weight distribution can be obtained by modifying commercially available polylactic acid resins. The modification can be achieved, for example, by introducing a crosslinked structure or a long-chain branched structure into the molecular structure of the polylactic acid resin. Alternatively, the modification can be achieved by increasing the molecular weight of the polylactic acid resin. A chain extender such as carbodiimide can be used to increase the molecular weight of the polylactic acid resin. Furthermore, modification with a chain extender can be achieved using a compound having one or more functional groups capable of undergoing a condensation reaction with hydroxyl or carboxyl groups present in the molecular structure of the polylactic acid resin, such as an acrylic organic compound, an epoxy organic compound, or an isocyanate organic compound. The modification can be achieved by bonding an acrylic organic compound, an epoxy organic compound, an isocyanate organic compound, or the like to the polylactic acid resin through a reaction.

[0057] Modification of polylactic acid resin through crosslinking or long-chain branching can be achieved, for example, by reacting polylactic acid resins with each other using a radical initiator. Among the above modification methods, reacting polylactic acid resins with each other using a radical initiator is preferred because it can prevent the inclusion of other components in the polylactic acid resin foam sheet. Furthermore, when polylactic acid resins are reacted with each other in an extruder using a radical initiator with appropriate reactivity, sites of the polylactic acid resin that are prone to decomposition are attacked by free radicals generated by the radical initiator. These sites can then become crosslinking points (branching points) and be stabilized. Such modification of polylactic acid resin increases its thermal stability and makes it less susceptible to molecular weight degradation when passing through an extruder. Examples of radical initiators used to modify polylactic acid resin include organic peroxides, azo compounds, and halogen molecules. Among these, organic peroxides are preferred.

[0058] Examples of the organic peroxide used in this embodiment include peroxyesters, hydroperoxides, dialkyl peroxides, diacyl peroxides, peroxydicarbonates, peroxyketals, and ketone peroxides.

[0059] Examples of the peroxy ester include t-butylperoxy 2-ethylhexyl carbonate, t-hexylperoxy isopropyl monocarbonate, t-hexylperoxybenzoate, t-butylperoxybenzoate, t-butylperoxy laurate, t-butylperoxy-3,5,5-trimethylhexanoate, t-butylperoxy acetate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, and t-butylperoxy isopropyl monocarbonate.

[0060] Examples of the hydroperoxide include permethane hydroperoxide, diisopropylbenzene hydroperoxide, cumene hydroperoxide, and t-butyl hydroperoxide.

[0061] Examples of the dialkyl peroxide include dicumyl peroxide, di-t-butyl peroxide, and 2,5-dimethyl-2,5-di(t-butylperoxy)-hexyne-3.

[0062] Examples of the diacyl peroxide include dibenzoyl peroxide, di(4-methylbenzoyl) peroxide, and di(3-methylbenzoyl) peroxide.

[0063] Examples of the peroxydicarbonate include di(2-ethylhexyl) peroxydicarbonate and diisopropyl peroxydicarbonate.

[0064] Examples of the peroxyketal include 1,1-di-t-butylperoxy-3,3,5-trimethylcyclohexane, 1,1-di-t-butylperoxycyclohexane, 2,2-di(t-butylperoxy)-butane, n-butyl 4,4-di-(t-butylperoxy)valerate, and 2,2-bis(4,4-di-t-butylperoxycyclohexyl)propane.

[0065] Examples of the ketone peroxide include methyl ethyl ketone peroxide and acetylacetone peroxide.

[0066] Modification with the organic peroxide may result in the modified polylactic acid resin being contaminated with components having excessively large molecular weights that will gel when thermally melted, or may cause odor problems due to the decomposition residues of the organic peroxide.

[0067] The gel contained in the polylactic acid resin can cause the formation of coarse bubbles or microprotrusions in the foam layer. The gel content (gel fraction) of the polylactic acid resin or resin composition is preferably 4% by mass or less, more preferably 3% by mass or less, and even more preferably 2% by mass or less. The gel content (gel fraction) of the polylactic acid resin or resin composition can be determined using the apparatus shown in Figure 3 and the method described below.

[0068] <Method for Measuring Gel Content> The pellets are used as samples. Approximately 0.5 g of sample is prepared, and the initial mass (m0 (g)) of this sample is precisely weighed. A 200-mesh wire mesh (wire diameter φ0.05 mm) is also prepared for filtering the solution in which the sample is dissolved. The initial mass (M0 (g)) of this wire mesh is also precisely weighed. The weighed measurement sample is placed in a 100 mL beaker (TB in Figure 3). 50 mL of chloroform as a solvent and a stirrer are placed in the beaker, and the beaker is covered with aluminum foil. Stirring is performed with a stirrer bar for 2 hours to dissolve the measurement sample at room temperature. After 2 hours, the aluminum foil is removed, and the solution in the beaker is filtered through a 200-mesh wire mesh. After filtration, the wire mesh is air-dried in a draft for 24 hours. After drying, it is cooled in a desiccator. After cooling, the wire mesh (M1 (g)) to which the resin insoluble matter adheres is weighed, and the gel fraction is calculated using the following formula. Gel fraction (mass%) = m1 / m0 x 100 m0: initial mass of sample m1: mass of insoluble resin (M1-M0) M0: initial mass of wire mesh M1: total mass of insoluble resin and wire mesh

[0069] The organic peroxide is preferably a peroxyester, since it can suppress the risk of gel formation and can easily modify the polylactic acid resin to a state suitable for foaming. Furthermore, among peroxyesters, the organic peroxide used to modify the polylactic acid resin is preferably a peroxycarbonate-based organic peroxide such as peroxymonocarbonate or peroxydicarbonate. In this embodiment, the organic peroxide used to modify the polylactic acid resin is preferably a peroxymonocarbonate-based organic peroxide, and particularly preferably t-butylperoxyisopropylmonocarbonate.

[0070] The organic peroxides described above are typically used in an amount of 0.1 parts by mass or more per 100 parts by mass of the polylactic acid resin to be modified, depending on factors such as the molecular weight. The amount of organic peroxide used is preferably 0.2 parts by mass or more, and particularly preferably 0.3 parts by mass or more. The amount of organic peroxide used is preferably 2.0 parts by mass or less, more preferably 1.5 parts by mass or less, and particularly preferably 1.0 part by mass or less.

[0071] By modifying polylactic acid resin using organic peroxide in such a ratio, the modified polylactic acid resin can be made suitable for foaming. When the amount of organic peroxide used is 0.1 parts by mass or more, the effect of modifying the polylactic acid resin is more reliably exerted. Furthermore, when the amount of organic peroxide used is 2.0 parts by mass or less, the modified polylactic acid resin is less likely to contain gel.

[0072] The polylactic acid resin of this embodiment can have a gel fraction of, for example, 1.5% by mass or less by using multiple polylactic acid resins with different MFRs as starting materials. When multiple polylactic acid resins with different MFRs are used as starting materials, the gel fraction can be 1.0% by mass or less, or even 0.8% by mass or less.

[0073] Examples of foaming components used when the polylactic acid resin is extruded into an extruded foam sheet include a foaming agent and a cell regulator.

[0074] As the blowing agent, a common blowing agent can be used, including a volatile blowing agent that becomes a gas at room temperature (23°C) and normal pressure (1 atmosphere) and a decomposition-type blowing agent that generates a gas by thermal decomposition. Examples of the volatile blowing agent that can be used include inert gases, aliphatic hydrocarbons, and alicyclic hydrocarbons. Examples of the inert gas include carbon dioxide and nitrogen. Examples of the aliphatic hydrocarbons include propane, normal butane, isobutane, normal pentane, and isopentane. Examples of the alicyclic hydrocarbons include cyclopentane and cyclohexane. In this embodiment, normal butane and isobutane are particularly preferred among the above.

[0075] Examples of the decomposition type foaming agent include azodicarbonamide, dinitrosopentamethylenetetramine, sodium bicarbonate, and a mixture of an organic acid such as citric acid or a salt thereof with a bicarbonate.

[0076] Examples of the foam regulator include polytetrafluoroethylene, talc, aluminum hydroxide, silica, etc. The decomposition type foaming agent can be used in combination with a volatile foaming agent to regulate the foam state, and can also be used as a foam regulator.

[0077] Various additives can be added to the resin composition constituting the polylactic acid resin foam sheet as needed. Examples of such additives include resins other than polylactic acid resin, inorganic fillers, and various chemicals. Examples of such chemicals include nucleating agents, lubricants, antioxidants, antistatic agents, flame retardants, UV absorbers, light stabilizers, colorants, and antibacterial agents. The proportion of these additives in the resin composition is preferably 25 parts by weight or less, and more preferably 15 parts by weight or less, per 100 parts by weight of polylactic acid resin.

[0078] The resin composition preferably contains a nucleating agent. The nucleating agent is preferably a substance that functions like a plasticizer and can promote the crystallization of polylactic acid. As such a nucleating agent, a reaction product (A) of (A1) at least one of a polyol and a polyol dehydration condensate, (A2) an alkylene oxide mainly composed of ethylene oxide, and (A3) a fatty acid having 12 to 24 carbon atoms is used.

[0079] Examples of the polyol in (A1) "polyol and polyol dehydration condensate" include glycerin, erythritol, pentaerythritol, xylitol, sorbitol, mannitol, galactitol, and maltitol. These are advantageous in imparting impact resistance to the polylactic acid resin foam sheet.

[0080] The above (A2) "alkylene oxide mainly composed of ethylene oxide" means that the majority of the alkylene oxide is ethylene oxide, and also includes alkylene oxides in which all of the alkylene oxide is ethylene oxide. When an alkylene oxide other than ethylene oxide is used in combination with ethylene oxide, for example, propylene oxide, butylene oxide, isobutylene oxide, etc. are used in combination.

[0081] Examples of (A3) "fatty acids having 12 to 24 carbon atoms" include saturated fatty acids such as dodecanoic acid (lauric acid), tetradecanoic acid (myristic acid), pentadecanoic acid (pentadecylic acid), hexadecanoic acid (palmitic acid), heptadecanoic acid (margaric acid), octadecanoic acid (stearic acid), icosanoic acid (arachidic acid), heneicosanoic acid (henicosylic acid), docosanoic acid (behenic acid), and tetracosanoic acid (lignoceric acid); and monounsaturated fatty acids such as myristoleic acid, palmitoleic acid, sapienic acid, oleic acid, elaidic acid, vaccenic acid, gadoleic acid, eicosenoic acid, and erucic acid. (A3) "fatty acids having 12 to 24 carbon atoms" may be diunsaturated fatty acids such as linoleic acid, triunsaturated fatty acids such as linolenic acid, or tetraunsaturated fatty acids or pentaunsaturated fatty acids. (A3) "C12-24 fatty acid" may be a mixture of multiple fatty acids such as coconut oil fatty acid. (A3) "C12-24 fatty acid" is preferably dodecanoic acid (lauric acid), octadecanoic acid (stearic acid), or the like.

[0082] In order to provide a polylactic acid resin foam sheet with excellent impact resistance, the reaction product (A) preferably has an oxyethylene group content of 20% by mass or more and 95% by mass or less. The oxyethylene group content of the reaction product (A) is more preferably 30% by mass or more and 95% by mass or less. The reaction product (A) may be either a saturated ester in which all hydroxyl groups of the polyol and polyol dehydration condensate are esterified with fatty acids, or a partial ester in which some of the hydroxyl groups are esterified. In order to provide a polylactic acid resin foam sheet with excellent impact resistance, the reaction product (A) preferably has an average number of ester groups per molecule. The average number of ester groups per molecule of the reaction product (A) is preferably more than 2 and not more than 9, more preferably more than 2.5 and not more than 6.

[0083] Examples of methods for producing the reaction product (A) include reacting a polyol with a fatty acid under heating to esterify the polyol, and then subjecting ethylene oxide to an addition reaction in an autoclave under heating to obtain the reaction product (A). Alternatively, a dehydration condensate of a polyol may be reacted with a fatty acid to esterify the polyol, followed by addition of ethylene oxide in the same manner as described above. Alternatively, ethylene oxide may be added to a polyol and a polyol dehydration condensate, followed by reaction with a fatty acid. Other methods include synthesizing a fatty acid ester in advance from a fatty acid and a monohydric alcohol with a short carbon number (methanol, ethanol), subjecting the ester exchange reaction with a polyol and a polyol dehydration condensate, and then adding ethylene oxide in the same manner as described above to obtain the reaction product (A). The reaction products (A) obtained in this manner may be used alone or in combination of two or more in the resin composition of this embodiment.

[0084] As the crystal nucleating agent of this embodiment, for example, the following "(B) fatty acid amide" may be used instead of the above-mentioned "(A) reaction product." As the crystal nucleating agent of this embodiment, one or more of the above-mentioned (A) reaction products and one or more of the (B) fatty acid amides may be used in combination.

[0085] The (B) fatty acid amide is, for example, at least one fatty acid amide selected from the group consisting of fatty acid monoamides, fatty acid bisamides, hydroxyl group-containing fatty acid monoamides, and hydroxyl group-containing fatty acid bisamides, and is preferably a fatty acid amide derived from a fatty acid having 8 to 24 carbon atoms. The (B) fatty acid amide is more preferably a fatty acid bisamide such as N,N'-ethylenebisstearamide, or a hydroxyl group-containing fatty acid bisamide such as N,N'-ethylenebis(12-hydroxystearamide) or N,N'-xylylenebis(12-hydroxystearamide). Fatty acid amides are effective in imparting excellent moldability to polylactic acid resin foam sheets. Fatty acid amides are also effective in imparting excellent heat resistance and impact resistance to sheet-molded articles.

[0086] Furthermore, examples of the crystal nucleating agent that can be used include hydrocarbons such as liquid paraffin, paraffin wax, and synthetic polyethylene wax; metallic soaps such as zinc stearate, calcium stearate, and magnesium stearate; ethylene glycol, diethylene glycol, and polyethylene glycols having a structure in which three or more ethylene glycols are condensed and polymerized; propylene glycol, dipropylene glycol, and polypropylene glycols having a structure in which three or more propylene glycols are condensed and polymerized; 1,3-butylene glycol, 1,4-butylene glycol, and polybutylene glycols which are polymers thereof; and polyglycerin, diglycerin, and polyglycerins having higher chain lengths.

[0087] The above-exemplified crystal nucleating agents, which function like plasticizers, can migrate to the surface layer of the polylactic acid resin foam sheet and exude from the surface, a phenomenon known as "bleed-out." In particular, fatty acid amides tend to bleed out of the polylactic acid resin foam sheet during thermoforming. While this is typically considered a problem, it can be advantageous in terms of providing adequate slippage between the sheet and the mold, thereby improving the thickness uniformity of the sheet. In other words, if adequate slippage is not achieved between the mold and the polylactic acid resin foam sheet, the polylactic acid resin foam sheet may be locally stretched, resulting in thin-walled areas in the sheet. On the other hand, using fatty acid amides as crystal nucleating agents can avoid such problems. Furthermore, the tendency to bleed out reduces the amount of the agent remaining in the sheet, thereby preventing further crystallization-induced distortion in the case of unintended heating of the sheet.

[0088] The nucleating agent can be used in a proportion of 0.5 parts by mass or more and 15 parts by mass or less per 100 parts by mass of polylactic acid resin. The proportion of the nucleating agent may be 1 part by mass or more, or 1.5 parts by mass or more. The proportion of the nucleating agent per 100 parts by mass of polylactic acid resin may be 10 parts by mass or less, or 5 parts by mass or less.

[0089] The polylactic acid resin foam sheet of this embodiment can be produced by carrying out a step of modifying polylactic acid resin using a twin-screw extruder or the like (modification step), and a step of extrusion-foaming a polylactic acid resin composition containing the modified polylactic acid resin through an extruder equipped with a circular die at its tip (extrusion-foaming step).

[0090] In the modification step, for example, a twin-screw extruder equipped with a granulation die (hot-cut die) may be used to pelletize the modified polylactic acid resin immediately after the modification step. The twin-screw extruder used in the modification step may be equipped with a strand die or T-die, and the modified polylactic acid resin may be formed into a strand or sheet in the modification step, followed by a separate step of cutting the strand or sheet and granulating it. Furthermore, as mentioned above, a tandem extruder may be used to perform an extrusion-foaming step immediately following the modification step.

[0091] In the extrusion foaming process described above, the resin composition of this embodiment does not easily stretch, and the resin film defining the cells is unlikely to become excessively thin. That is, in the polylactic acid resin foam sheet of this embodiment, the resin film containing the polylactic acid resin described above exhibits a certain level of resistance when stretched by the foaming force of the foaming agent. Furthermore, in the polylactic acid resin foam sheet of this embodiment, the resin film tends to be thin in the center and thick at the periphery. Therefore, the polylactic acid resin foam sheet of this embodiment exhibits excellent mechanical properties because the thick resin film is three-dimensionally connected throughout the entire sheet.

[0092] In the polylactic acid resin foam sheet of this embodiment, even if bubbles break during foaming and a hole is created in the resin film, the resin film surrounding the hole does not remain as it is but shrinks and increases in thickness in a manner that is effective in exhibiting strength, so that the sheet can exhibit excellent strength even if it has a certain proportion of open bubbles.

[0093] The apparent density of the polylactic acid resin foam sheet is preferably 63 kg / m 3 More than 500kg / m 3 More preferably, it is 83 kg / m or less. 3 More than 250kg / m 3 The apparent density of the polylactic acid resin foam sheet is 63 kg / m or less. 3 As a result of the above, the sheet molding of this embodiment has high strength, and further has the advantage that the thermoformability of the polylactic acid resin foam sheet is good, resulting in a molding that accurately reflects the shape of the mold.

[0094] The polylactic acid resin foam sheet has an apparent density of 500 kg / m 3 By satisfying the following conditions, there is an advantage that the sheet molding of this embodiment can easily exhibit the characteristics of a foam, such as light weight, heat insulating properties, and shock absorbing properties.

[0095] The thickness of the polylactic acid resin foam sheet is preferably 0.5 mm to 7 mm, more preferably 0.5 mm to 5 mm, and even more preferably 0.7 mm to 3 mm. Having a thickness of 0.5 mm or more provides the advantage of high strength for the sheet molding of this embodiment. Furthermore, having a thickness of 7 mm or less provides good thermoformability, resulting in less thickness unevenness for the sheet molding of this embodiment.

[0096] <Apparent density> Apparent density (kg / m) of polylactic acid resin foam sheet 3 ) is the mass of the polylactic acid resin foam sheet per unit area (basis weight: g / m 2 ) by the thickness (mm) of the polylactic acid resin foam sheet. The basis weight can be determined by arithmetically averaging the values ​​measured for a plurality of samples cut out from the polylactic acid resin foam sheet. The basis weight of the polylactic acid resin foam sheet is determined by cutting out a measurement sample from the polylactic acid resin foam sheet so that the dimension in the extrusion direction (MD) is 20 cm and the dimension in the transverse direction (TD) is the full width, and calculating the mass W (g) and area S (cm 2 ) and the basis weight (g / m 2 ) = W / S × 10000 Also, the apparent density can be calculated using the following formula: Apparent density (kg / m 3 )=Basic weight (g / m 2 ) ÷ thickness (mm)

[0097] <Thickness> The thickness of the polylactic acid resin foam sheet can be determined by, for example, taking an enlarged photograph of a cross section of the polylactic acid resin foam sheet cut along a plane perpendicular to the polylactic acid resin foam sheet, and is determined as the average value of multiple randomly selected points (e.g., 20 points).

[0098] The polylactic acid resin foam sheet preferably has a predetermined average cell diameter. The average cell diameter is preferably 0.1 mm to 1 mm, more preferably 0.1 mm to 0.8 mm, and even more preferably 0.1 mm to 0.6 mm. When the polylactic acid resin foam sheet has an average cell diameter of 0.1 mm or more, the open cell ratio tends to be low. As a result, it is possible to obtain a sheet molded body with a low apparent density. This also results in improved thermoformability of the polylactic acid resin foam sheet, which in turn results in reduced thickness unevenness of the sheet molded body. Furthermore, when the polylactic acid resin foam sheet has an average cell diameter of 1 mm or less, the sheet molded body of this embodiment has excellent properties such as heat insulation and cushioning. The average cell diameter of the sheet molded body of this embodiment is preferably the same as the average cell diameter of the polylactic acid resin foam sheet described above.

[0099] (Average Cell Diameter) The average cell diameter can be measured in accordance with the test method of ASTM D2842-69. Specifically, a polylactic acid resin foam sheet is cut along the extrusion direction (MD) and the width direction (TD) perpendicular to the extrusion direction, and the center of each cut surface is magnified and photographed at two different locations using a scanning electron microscope (S-3000N, manufactured by Hitachi, Ltd.). Next, the photographed images are printed on A4 paper, and three straight lines, each 60 mm long, are drawn on the images. Note that for the cut surface cut in the MD, straight lines are drawn parallel to the MD, and for the cut surface cut in the TD, straight lines are drawn parallel to the TD. Furthermore, for the thickness direction (VD), straight lines are drawn on one image each in the MD and TD. The magnification of the electron microscope is adjusted so that six or more bubbles are present on each straight line. Then, the average chord length (t) of the bubbles is calculated from the average number of bubbles present in each direction on the six straight lines drawn in each direction using the following formula, and the bubble diameter in each direction (MD, TD, VD) is calculated from this average chord length using the following formula: Average chord length t = 60 (mm) / (number of bubbles x magnification of photograph) Bubble diameter D = t / 0.616 (mm) Note that when drawing the straight lines, it is best to ensure that the straight lines penetrate the bubbles without making point contact with them. Furthermore, if some bubbles make point contact with the straight lines, these bubbles are also included in the number of bubbles. Furthermore, if both ends of the straight line are located within the bubbles without penetrating them, the bubbles where both ends of the straight line are located are also included in the number of bubbles. Then, the obtained bubble diameter (D) in MD is calculated. MD ) and bubble diameter at TD (D TD ) and bubble diameter at VD (D VD ) is defined as the average cell diameter of the polylactic acid resin foam sheet. That is, the average cell diameter of the polylactic acid resin foam sheet is calculated by the following formula: Average Cell Diameter (mm) = (D MD ×D TD ×D VD ) 1/3

[0100] The open cell ratio of the polylactic acid resin foam sheet is preferably 50% or less, more preferably 40% or less, and even more preferably 30% or less. Having an open cell ratio of 50% or less in the polylactic acid resin foam sheet has the advantage of providing particularly excellent mechanical strength and secondary foaming properties during thermoforming. Furthermore, a sheet molded product manufactured from such a polylactic acid resin foam sheet has excellent mechanical strength and also excellent appearance, such as mold reproducibility. In this embodiment, the open cell ratio of the sheet molded product itself is preferably the above-mentioned value. The open cell ratio can be determined as follows.

[0101] (Open Cell Ratio) The open cell ratio can be determined by the following method. A number of sheet-like samples measuring 25 mm long x 25 mm wide are cut out from a polylactic acid resin foam sheet. The cut-out samples are stacked together without leaving any gaps to form test pieces with a thickness of 21 to 23 mm. Three test pieces are prepared. The test pieces are conditioned for 16 hours in an environment of JIS K7100:1999, symbol 23 / 50, class 2, and the thickness (mm) is measured. For example, a "Digimatic Caliper" caliper manufactured by Mitutoyo Corporation can be used to measure the thickness. The thickness is measured to the nearest 1 / 100 mm, and the apparent volume (cm 3 Next, the volume (cm ) of the test piece is measured under the above environment using a dry automatic density meter (for example, "Accupyk II 1340-100cc" manufactured by Shimadzu Corporation). 3 ) is measured under the following measurement conditions: Gas used: Nitrogen Container used: 35 cc Filling pressure: 0.005 psig End rate of pressure equilibrium: 0.005 psig / min Number of repetitions: 1 Then, the open cell rate (%) of each test piece is calculated using the following formula, and the average value is taken as the apparent density of the polylactic acid resin foam sheet. Open cell rate (%) = [(apparent volume - volume measured with a dry automatic density meter) / apparent volume] x 100 (%)

[0102] Next, a method for producing a sheet molded body of this embodiment will be described. The method for producing a sheet molded body of this embodiment includes a primary heating step of heating the polylactic acid resin foam sheet, and a secondary heating step of sandwiching the polylactic acid resin foam sheet that has been subjected to the primary heating step between heated molds to produce a sheet molded body and increase the crystallinity of the sheet molded body.

[0103] In the primary heating step, the polylactic acid resin foam sheet can be heated by a known method, such as sandwiching the polylactic acid resin foam sheet between heating plates or heating the foam sheet with an electric heater. In the primary heating step of the method for producing a sheet molded product of this embodiment, the polylactic acid resin foam sheet is heated to a surface temperature of preferably 60° C. or higher, more preferably 70° C. or higher, even more preferably 80° C. or higher, and particularly preferably 90° C. or higher. Heating in the primary heating step is preferably carried out so that the surface temperature of the polylactic acid resin foam sheet is 130° C. or lower, and more preferably 120° C. or lower.

[0104] In the method for producing a sheet molded body of this embodiment, the surface temperature of the polylactic acid resin foam sheet in the primary heating step is set to the above-mentioned temperature, thereby improving the transferability of the molding die. Furthermore, performing the primary heating step at the above-mentioned temperature improves the softening state of the polylactic acid resin foam sheet, thereby preventing the polylactic acid resin foam sheet from breaking during molding. Furthermore, in the method for producing a sheet molded body of this embodiment, the surface temperature of the polylactic acid resin foam sheet in the primary heating step is set to preferably 130°C or less, more preferably 120°C or less, thereby improving the surface condition of the polylactic acid resin foam sheet. Furthermore, performing the primary heating step at such a temperature promotes moderate crystallization during the primary heating step, increasing the crystallinity of the resulting sheet molded body and making it easier to obtain a sheet molded body with excellent heat resistance.

[0105] In the secondary heating step, a pair of male and female molds is preferably used as the molding die. In the secondary heating step, the polylactic acid resin foam sheet heated and softened in the primary heating step is sandwiched between the heated male and female molds to form a sheet molded body. In the secondary heating step, this state is maintained for a certain period of time, so that the crystallinity of the sheet molded body can be increased over time.

[0106] The secondary heating step is carried out by adjusting the temperature of the mold to preferably 50°C or higher, more preferably 60°C or higher, and even more preferably 70°C or higher. The secondary heating step is carried out by adjusting the temperature of the mold to preferably 130°C or lower, more preferably 120°C or lower. By adjusting the temperature of the mold to 50°C or higher in the secondary heating step, the crystallinity of the sheet-molded body is advantageously increased. Furthermore, by adjusting the temperature of the mold to 50°C or higher in the secondary heating step, the time required for crystallization can be shortened, which also makes it easier to increase productivity. Furthermore, by adjusting the heated mold to 130°C or lower in the secondary heating step, the surface condition of the sheet-molded body is advantageously improved.

[0107] In the method for producing a sheet molded body of this embodiment, it is preferable to adjust the temperature of the polylactic acid resin foam sheet obtained by the extrusion foaming method immediately after extrusion, from the viewpoint of obtaining a polylactic acid resin foam sheet in which the difference between the heat absorption and heat generation is within a preferred range. The temperature adjustment method can be, for example, a method of cooling with air or water, or a method of keeping the sheet warm (heating) with heated air or hot water. The sheet molded body formed by the method for producing a sheet molded body of this embodiment has excellent heat resistance. Because of its excellent heat resistance, the sheet molded body of this embodiment can be suitably used as a food packaging container such as a lunch box, a cup noodle container, or a microwaveable container.

[0108] The above-mentioned examples of the polylactic acid resin foam sheet and the sheet molded product, and the manufacturing method thereof, according to the present embodiment are merely restrictive examples, and the present invention is not limited to the above-mentioned examples and can be carried out by making appropriate modifications to the above-mentioned examples. As described above, the present embodiment includes the following disclosures.

[0109] (1) A polylactic acid resin foam sheet composed of a polylactic acid resin composition containing a crystalline polylactic acid resin, the polylactic acid resin foam sheet having a degree of crystallinity of 30% or less and a crystallization temperature of 105°C or less as measured by heat flux differential scanning calorimetry at a heating rate of 5°C / min.

[0110] (2) The polylactic acid resin foam sheet according to (1), wherein the polylactic acid resin composition has a semi-crystallization time of 30 minutes or less at 80°C.

[0111] (3) The polylactic acid resin foam sheet according to (1) or (2), wherein the polylactic acid resin composition contains the polylactic acid resin, which is a copolymer of D- and L-lactic acid, and the content of the D-form in the copolymer is 0.5 mol % or more and 5 mol % or less, and the melting point of the copolymer is 130°C or more and 170°C or less.

[0112] (4) Apparent density is 63 kg / m 3 More than 500kg / m 3 A polylactic acid resin foam sheet according to any one of (1) to (3) below.

[0113] (5) The polylactic acid resin foam sheet according to any one of (1) to (4), having a thickness of 0.5 mm or more and 7 mm or less.

[0114] (6) The polylactic acid resin foam sheet according to any one of (1) to (5), having an open cell ratio of 50% or less.

[0115] (7) The polylactic acid resin foam sheet according to any one of (1) to (6), wherein the polylactic acid resin composition contains a modified polylactic acid resin, which is a product modified with an organic peroxide, as the polylactic acid resin.

[0116] (8) The polylactic acid resin foam sheet according to any one of (1) to (7), wherein the polylactic acid resin composition contains a crystal nucleating agent.

[0117] (9) A method for producing a sheet molded body by thermoforming a resin foam sheet, wherein the resin foam sheet is a polylactic acid resin foam sheet made of a polylactic acid resin composition containing a crystalline polylactic acid resin, the resin foam sheet having a crystallinity of 30% or less and a crystallization temperature of 105°C or less as observed by heat flux differential scanning calorimetry at a heating rate of 5°C / min, the method comprising: a primary heating step of heating the polylactic acid resin foam sheet; and a secondary heating step of sandwiching the polylactic acid resin foam sheet subjected to the primary heating step between heated molds to produce a sheet molded body and increase the crystallinity of the sheet molded body.

[0118] (10) The method for producing a sheet molded body according to (9), wherein in the primary heating step, the polylactic acid resin foam sheet is heated so that the surface temperature becomes 60°C or higher and 130°C or lower.

[0119] (11) The method for producing a sheet molded body according to (9) or (10), wherein the temperature of the mold is adjusted to 50° C. or higher and 130° C. or lower in the secondary heating step.

[0120] According to the invention as described above, a polylactic acid resin foam sheet suitable for efficiently producing a sheet molding having excellent heat resistance is provided, and the production efficiency of a sheet molding having excellent heat resistance can be improved.

[0121] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. (Reference Production Example 1) (1) Preparation of modified polylactic acid resin Polylactic acid resin (MFR = 10.0 g / 10 min, density = 1240 kg / m 3) and 0.5 parts by mass of t-butylperoxyisopropyl monocarbonate (1-minute half-life temperature T1: 158.8°C) were mixed and stirred in a ribbon blender to obtain a mixture. The resulting mixture was fed into a twin-screw extruder (L / D = 31.5) with a diameter of 57 mm. The feed section was set to a temperature of 170°C, the temperature thereafter to 230°C, and the mixture was melt-kneaded in the twin-screw extruder at a rotation speed of 150 rpm. The kneaded material was extruded into strands at a discharge rate of 50 kg / h from a die with a diameter of 3 mm and 18 holes attached to the tip of the extruder. The extruded strand-like kneaded material was then passed through a 2-m-long cooling water tank containing water at 30°C and cooled. The cooled strands were cut with a pelletizer to obtain pellets of modified polylactic acid resin.

[0122] (Reference Production Examples 2 to 5) In Reference Production Examples 2 to 5, modified polylactic acid resins were prepared in the same manner as in Reference Production Example 1, except that the type of polylactic acid resin and the amount of organic peroxide added (amount added (parts by mass) per 100 parts by mass of polylactic acid resin) were changed.

[0123] (Reference Examples 1 and 2) Reference Examples 1 and 2 are commercially available polylactic acid resins, which are raw materials before the above-described reactions. Table 1 shows the types of polylactic acid resins and organic peroxides used in Reference Production Examples 1 to 5, the amounts (parts by mass) of organic peroxides added per 100 parts by mass of polylactic acid resin, and the physical properties of the resulting polylactic acid resins.

[0124]

[0125] (Preparation of Polylactic Acid Foam Sheet) (Example 1) 100 parts by mass of the polylactic acid resin obtained in Reference Production Example 1 and 1.0 part by mass of a cell control agent ("Crown Talc" manufactured by Matsumura Sangyo Co., Ltd.) were dry blended to prepare a mixture. The mixture was supplied through a hopper to the first extruder (diameter φ50 mm) of a tandem extruder equipped with a first extruder (upstream side) with a diameter of φ50 mm and a second extruder (downstream side) with a diameter of φ65 mm, and heated and melted in the first extruder. Then, butane (isobutane / normal butane = 70 / 30) as a foaming agent was pressure-fed into the first extruder and melt-mixed with the mixture. The molten mixture was then transferred to a second extruder with a diameter of 65 mm and uniformly cooled to a temperature suitable for extrusion foaming. After that, the mixture was extruded and foamed through a circular die with a diameter of 70 mm at a discharge rate of 30 kg / h to obtain a cylindrical foam. The obtained cylindrical foam was placed on a φ206 mm mandrel whose inside was cooled with water at approximately 20°C, and its outer surface was cooled and molded by blowing air onto it using an air ring larger than its diameter.The foam was then cut open at one point on the circumference using a cutter to obtain a strip-shaped polylactic acid resin foam sheet.

[0126] Example 2 A polylactic acid resin foam sheet was obtained in the same manner as in Example 1, except that 10 parts by mass of a crystal nucleating agent (manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd., trade name "TRIBIO S-920MB") was added per 100 parts by mass of the polylactic acid resin.

[0127] Example 3 A polylactic acid resin foam sheet was obtained in the same manner as in Example 1, except that 2 parts by mass of a nucleating agent (manufactured by Ito Oil Mills, trade name "ITOHWAX J-530" (fatty acid amide)) was added per 100 parts by mass of the polylactic acid resin.

[0128] Example 4 A polylactic acid resin foam sheet was obtained in the same manner as in Example 3, except that the polylactic acid resin used was changed to that obtained in Reference Production Example 2.

[0129] Example 5 A polylactic acid resin foam sheet was obtained in the same manner as in Example 3, except that the amount of the nucleating agent added was changed from 2 parts by mass to 3 parts by mass.

[0130] Example 6 A polylactic acid resin foam sheet was obtained in the same manner as in Example 1, except that 3 parts by mass of polyethylene glycol (PEG-4000P) was added as a nucleating agent relative to 100 parts by mass of the polylactic acid resin.

[0131] Example 7 A polylactic acid resin foam sheet was obtained in the same manner as in Example 1, except that a combination of product names "ITOHWAX J-530" and "PEG-4000P" was used as a nucleating agent, and the amount of each added was 3 parts by mass (6 parts by mass in total) per 100 parts by mass of the polylactic acid resin.

[0132] Example 8 A polylactic acid resin foam sheet was obtained in the same manner as in Example 1, except that the polylactic acid resin used was changed to that obtained in Reference Production Example 3.

[0133] Example 9 A polylactic acid resin foam sheet was obtained in the same manner as in Example 3, except that the polylactic acid resin used was changed to that obtained in Reference Production Example 4.

[0134] Comparative Example 1 A polylactic acid resin foam sheet was obtained in the same manner as in Example 1, except that a combination of trade names "ITOHWAX J-530" and "PEG-4000P" was used as a nucleating agent, and the amount of "ITOHWAX J-530" added was 1 part by mass and the amount of "PEG-4000P" added was 4 parts by mass relative to 100 parts by mass of the polylactic acid resin.

[0135] Comparative Example 2 A polylactic acid resin foam sheet was obtained in the same manner as in Example 1, except that the polylactic acid resin used was changed to that obtained in Reference Production Example 4.

[0136] Comparative Example 3 A polylactic acid resin foam sheet was obtained in the same manner as in Example 1, except that the polylactic acid resin used was changed to that obtained in Reference Production Example 5.

[0137] (Comparative Examples 4 and 5) An attempt was made to produce a polylactic acid resin foam sheet in the same manner as in Example 1, except that the polylactic acid resin used was that of Reference Example 1 (Comparative Example 4) or Reference Example 2 (Comparative Example 5). However, the melt tension of the resin was low, and a polylactic acid resin foam sheet in a good condition could not be obtained.

[0138] <Molding> Planar square test pieces measuring 340 mm long x 340 mm wide were cut out from the polylactic acid resin foam sheet of each example. A single-shot molding machine (manufactured by Tosei Sangyo Co., Ltd., product name "FM-3A") was used, and the average temperature of the upper heater of this single-shot molding machine was set to 300°C, and the average temperature of the lower heater was set to 300°C. Next, the test pieces were introduced into the single-shot molding machine and heated for 30 seconds. Five sheet-shaped molded bodies (foam containers) having an opening at the top were produced by thermoforming using a mold heated and maintained at 100°C for each example. Note that the surface temperature of the polylactic acid resin foam sheet during the primary heating step under the above conditions was approximately 120°C. The containers were in the shape of an inverted truncated pyramid with a square bottom, and the dimensions of each part were as follows: Opening: 140 mm x 150 mm; Bottom: 110 mm x 110 mm; Height: 60 mm

[0139] The crystallinity and shrinkage upon heating (hereinafter referred to as heat shrinkage) of each of the resulting containers were measured. The shrinkage upon heating was measured by the following method.

[0140] (Heat shrinkage rate) An air-circulating oven, for example, a product name "MODEL PSL-2" manufactured by Tabai Espec Corporation, was used to measure the heat shrinkage rate. Each of the obtained containers was placed in an air-circulating oven heated to 100°C and heated for 150 seconds, then removed from the oven and the length of each side of the container was measured, and the heat shrinkage rate was calculated from these measurements. The heat shrinkage rate of the container was calculated by dividing the difference between the length before and after heating by the length before heating and multiplying the result by 100, and was calculated for each of the two sides of the opening of the container. Based on the calculated values, evaluation was performed according to the following evaluation criteria.

[0141] <Evaluation criteria> ◯: Both sides were "within 5%". △: One side was "within 5%" and the other side was "more than 5%". ×: Both sides were "more than 5%".

[0142] The thickness, basis weight, expansion ratio, open cell ratio, average cell diameter, crystallinity, crystallization temperature, and half-crystallization time of the polylactic acid resin foam sheets of the Examples and Comparative Examples were measured. The expansion ratio was measured by the following method. The other items were measured by the methods described above.

[0143] (Expansion Ratio) Three 10 x 10 cm measurement samples were cut out from the polylactic acid resin foam sheet in the transverse direction (TD), and the thickness and mass of each sample were measured. The arithmetic mean value of the densities calculated from the mass and volume of each sample was used as the apparent density of the polylactic acid resin foam sheet. 3 The value obtained by dividing the apparent density of the polylactic acid resin foam sheet by the apparent density of the polylactic acid resin foam sheet was taken as the expansion ratio. Expansion ratio = 1240 / apparent density of polylactic acid resin foam sheet (kg / m 3 )

[0144] The results are shown in Tables 2 and 3 below.

[0145]

[0146]

[0147] From the above, it can be seen that the present invention can provide a polylactic acid resin foam sheet suitable for efficiently producing a sheet molding having excellent heat resistance.

[0148] 1: Polylactic acid resin foam sheet, 100: Sheet manufacturing apparatus

Claims

1. A polylactic acid resin foam sheet composed of a polylactic acid resin composition containing a crystalline polylactic acid resin, the polylactic acid resin foam sheet having a degree of crystallinity of 30% or less and a crystallization temperature of 105°C or less as observed by heat flux differential scanning calorimetry at a heating rate of 5°C / min.

2. The polylactic acid resin foam sheet according to claim 1, wherein the polylactic acid resin composition has a semi-crystallization time at 80° C. of 30 minutes or less.

3. A polylactic acid resin foam sheet according to claim 1 or 2, wherein the polylactic acid resin composition contains the polylactic acid resin which is a copolymer in which D- and L-forms of lactic acid are copolymerized, the content of the D-form in the copolymer is from 0.5 mol % to 5 mol %, and the melting point of the copolymer is from 130°C to 170°C.

4. Apparent density is 63 kg / m 3 More than 500kg / m 3 3. The polylactic acid resin foam sheet according to claim 1, wherein:

5. The polylactic acid resin foam sheet according to claim 1 or 2, which has a thickness of 0.5 mm or more and 7 mm or less.

6. The polylactic acid resin foam sheet according to claim 1 or 2, which has an open cell ratio of 50% or less.

7. The polylactic acid resin foam sheet according to claim 1 or 2, wherein the polylactic acid resin is a modified polylactic acid resin which is modified with an organic peroxide.

8. The polylactic acid resin foam sheet according to claim 1 or 2, wherein the polylactic acid resin composition contains a crystal nucleating agent.

9. A method for producing a sheet molded body by thermoforming a resin foam sheet, wherein the resin foam sheet is a polylactic acid resin foam sheet composed of a polylactic acid resin composition containing a crystalline polylactic acid resin, and has a crystallinity of 30% or less and a crystallization temperature of 105°C or less as observed by heat flux differential scanning calorimetry at a heating rate of 5°C / min, the method comprising the steps of: a primary heating step of heating the polylactic acid resin foam sheet; and a secondary heating step of sandwiching the polylactic acid resin foam sheet after the primary heating step between a heated mold to produce a sheet molded body and increase the crystallinity of the sheet molded body.

10. The method for producing a sheet molded body according to claim 9, wherein in the primary heating step, the polylactic acid resin foam sheet is heated so that the surface temperature is 60°C or higher and 130°C or lower.

11. The method for producing a sheet molded body according to claim 9 or 10, wherein in the secondary heating step, the temperature of the mold is adjusted to 50°C or higher and 130°C or lower.

Citation Information

Patent Citations

  • Polylactic acid-based resin foam molded product

    JP5517280B2

  • Polylactic acid-based resin foam

    JP2009068021A

  • Method of manufacturing polyester based resin foamed molding, and polyester based resin foamed molding

    JP2012020444A

  • Polylactic acid-based resin foam, and polylactic acid-based foam molded body

    JP2012077150A

  • Polylactic acid-based resin-foamed sheet molding, and method for producing the same

    JP2014139333A