Laminate and method for producing laminate

The laminate with regular and irregular resin particle arrangements and coating layers addresses the issues of contrast, gloss, and abrasion resistance in structural color laminates, enhancing their visibility and durability.

WO2024204560A1PCT designated stage expired Publication Date: 2024-10-03TOYO INK MFG CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012696
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing structural color laminates face issues with contrast, gloss, and abrasion resistance due to cracks and uneven scattering, particularly when heat-treated, which affect the visibility and durability of the structural colors.

Method used

A laminate with a pattern part A showing structural color and a pattern part B not showing structural color, where resin fine particles are regularly arranged in part A and irregularly in part B, along with a coating layer, to enhance contrast and gloss, and improve abrasion resistance.

Benefits of technology

The laminate achieves excellent contrast and gloss between structural and non-structural color portions while maintaining abrasion resistance by regular and irregular particle arrangements and coating layers, reducing unnecessary scattering and maintaining color intensity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

Provided is a laminate excellent in: glossiness; abrasion resistance; and contrast between a part showing structural colors and a part not showing structural colors. This laminate has, on a base material, a pattern part A showing structural colors and a pattern part B showing no structural colors. In the pattern part A, fine resin particles are regularly arranged, and in the pattern part B, fine resin particles are irregularly present.
Need to check novelty before this filing date? Find Prior Art

Description

Laminate and method for manufacturing laminate

[0001] The present disclosure relates to a laminate and a method for manufacturing the laminate.

[0002] The colors of living creatures, including Morpho butterflies and jewel beetles, are called structural colors, and are produced by the diffraction and interference of light due to regular structures with spacing similar to the wavelength of light. Structural colors are characterized by their vivid coloring and angular dependence, where the color changes depending on the angle from which it is observed, and can create an unprecedented sense of luxury and splendor. In recent years, the use of artificial structural colors has become popular, and they are used, for example, to decorate the back of smartphones and for sticker labels. For these applications, there is a demand for pattern formation technology using structural colors, which allows for the expression of only desired characters or images using structural colors.

[0003] Colloidal crystals are a type of structural color material with a structure in which particles are regularly and closely packed. The difference in refractive index between the particles and the spaces between them causes Bragg reflection, resulting in structural color. Among structural color materials, colloidal crystals are characterized by a narrow half-width and high-intensity reflection peak due to the regularity of the particles, resulting in a single, vivid structural color. Another feature is their ease of fabrication, which can be achieved by applying a particle suspension to a substrate and then drying. However, it is known that attempts to form colloidal crystals at practical production speeds result in considerable cracking during drying.

[0004] A known technique for forming patterns from structural color materials using colloidal crystals is to partially apply heat to fill the voids between the particles, thereby fading the structural color.

[0005] Patent Documents 1 and 2 disclose colloidal crystal laminates with heat-sensitive properties, and state that the structural color can be faded by heat treatment using a laser or the like, thereby forming an image. Colloidal crystal laminates develop color due to the difference in refractive index between the microparticles and their voids, and the structural color fades when the voids are filled by heat treatment. However, as described in Patent Documents 1 and 2, simply performing heat treatment fills the voids while maintaining the regular arrangement of the microparticles, which may result in insufficient contrast and reduced contrast due to cracks occurring in the treated area. Furthermore, the presence of these cracks causes unnecessary scattering, reducing the gloss of the heat-treated area.

[0006] JP 2022-80205 A

[0007] The problem to be solved by the present disclosure is to provide a laminate that is excellent in contrast between a portion exhibiting a structural color and a portion not exhibiting a structural color, gloss, and abrasion resistance.

[0008] As a result of extensive research into the above-mentioned problems, the inventors have found that the above-mentioned problems can be solved by using the laminate and the method for manufacturing the laminate described below, and have thus completed the present invention.

[0009] That is, the present disclosure relates to the following [1] to

[12] .

[0010] [1] A laminate having, on a substrate, a pattern portion A that exhibits structural color and a pattern portion B that does not exhibit structural color, wherein resin fine particles are regularly arranged in the pattern portion A and irregularly arranged in the pattern portion B.

[0011] [2] The laminate according to [1], wherein the film thickness of the pattern portion A is 5 to 30 μm.

[0012] [3] The laminate according to [1] or [2], wherein the pattern portion A exhibits a reflection peak having a half-width of less than 100 nm and a reflected light intensity of 5% or more in a wavelength range of 380 nm to 2000 nm when the diffuse reflectance spectrum is measured at an incident angle of 5°.

[0013] [4] The laminate according to any one of [1] to [3], wherein the pattern portion B does not exhibit a reflection peak having a half-width of less than 100 nm and a reflected light intensity of 5% or more in the wavelength range of 380 nm to 2000 nm when the diffuse reflectance spectrum is measured at an incident angle of 5°.

[0014] [5] The laminate according to any one of [1] to [4], further comprising a coating layer on the pattern portion A and / or the pattern portion B.

[0015] [6] The laminate according to [5], wherein the coating layer has a thickness of 0.1 to 10 μm.

[0016] [7] The laminate according to [5] or [6], wherein the coating layer contains a colorant.

[0017] [8] The laminate according to any one of [5] to [7], having a coating layer C containing a resin on the pattern portion B.

[0018] [9] The laminate according to any one of [5] to [8], having a coating layer D containing a resin on the pattern portion A.

[0019]

[10] The laminate according to [8], wherein the coating layer C contains a non-aqueous resin.

[0020]

[11] The laminate according to [9], wherein the coating layer D contains an aqueous resin.

[0021]

[12] The laminate according to any one of [1] to [4], having a coating layer C containing a non-aqueous resin on the pattern portion B, and a coating layer D containing an aqueous resin on the pattern portion A.

[0022]

[13] A method for manufacturing a laminate having, on a substrate, a pattern portion A that exhibits structural color and a pattern portion B that does not exhibit structural color, the method comprising: step 1 of applying a coating agent containing resin microparticles to the substrate to form pattern portion A that exhibits structural color due to a regular arrangement of the resin microparticles; and step 2 of applying a coating agent that does not contain resin microparticles to a part of pattern portion A to change pattern portion A to pattern portion B that does not exhibit structural color.

[0023] The present disclosure can provide a laminate that is excellent in contrast between a portion exhibiting a structural color and a portion not exhibiting a structural color, gloss, and abrasion resistance.

[0024] The following describes in detail the embodiments of the present invention. However, the following description of the constituent elements is an example of an embodiment of the present invention, and the present invention is not limited to these contents as long as it does not deviate from the gist of the present invention.

[0025] <Laminate> The laminate of the present disclosure is a laminate having, on a substrate, a pattern portion A that exhibits structural color and a pattern portion B that does not exhibit structural color, in which resin fine particles are regularly arranged in the pattern portion A and in which resin fine particles are irregularly arranged in the pattern portion B.

[0026] In pattern portion A, the resin microparticles are regularly arranged, resulting in a structural color with excellent color development, while in pattern portion B, the resin microparticles are irregularly arranged, resulting in fewer cracks in the coating film and a smoother coating, reducing unnecessary scattering. Due to the above effects, it is believed that the laminate of the present disclosure can achieve high levels of contrast and gloss. Note that this explanation is based solely on technical considerations and does not limit the invention in any way.

[0027] The laminate of the present disclosure preferably has a coating layer on the pattern portion A and / or the pattern portion B. In the present disclosure, the coating layer located on the pattern portion A is referred to as coating layer D, and the coating layer located on the pattern portion B is referred to as coating layer C.

[0028] <Layer Structure> Specific examples of the structure of the laminate of the present disclosure include, but are not limited to, the following structures. In the structure descriptions (1) to (8) below, " / " indicates the boundary between layers. Furthermore, although pattern portion A and pattern portion B may both exist on a single substrate, for the sake of clarity, the structure is described as being divided into pattern portion A and pattern portion B.

[0029] (1) Substrate / pattern portion A, pattern portion B (2) Substrate / pattern portion A, pattern portion B / coating layer C (on pattern portion B) (3) Substrate / pattern portion A, pattern portion B / coating layer D (on pattern portion A) (4) Substrate / pattern portion A, pattern portion B / coating layer C (on pattern portion B), coating layer D (on pattern portion A) (5) Substrate / primer layer / pattern portion A, pattern portion B (6) Substrate / primer layer / pattern portion A, pattern portion B / coating layer C (on pattern portion B) (7) Substrate / primer layer / pattern portion B / coating layer D (on pattern portion A) (8) Substrate / primer layer / pattern portion A, pattern portion B / coating layer C (on pattern portion B), coating layer D (on pattern portion A)

[0030] <Pattern portion A> In the present disclosure, the pattern portion A has a structure in which resin fine particles are regularly arranged. As a result, Bragg reflection occurs due to the difference in refractive index between the densely packed particles and the gaps between the particles, resulting in a vivid structural color. The resin fine particles present in the pattern portion A are preferably spherical.

[0031] The film thickness of the pattern portion A is preferably 5 to 30 μm, more preferably 7 to 20 μm, and even more preferably 8 to 15 μm. When the film thickness of the pattern portion A is 5 μm or more, excellent structural color is exhibited, resulting in good contrast with the non-structural color portion. Furthermore, when the film thickness is 30 μm or less, the strength of the pattern portion A is maintained, resulting in good abrasion resistance of the laminate.

[0032] When the diffuse reflectance spectrum of the pattern portion A is measured at an incident angle of 5°, it is preferable that the pattern portion A has a reflection peak in the wavelength range of 380 nm to 2000 nm, with a half-width of less than 100 nm and a reflected light intensity of 5% or more. The wavelength range of the reflection peak is more preferably 380 nm to 700 nm, the half-width is more preferably less than 60 nm, and the reflected light intensity is more preferably 10% or more.

[0033] When the pattern portion A exhibits the above optical properties, an excellent structural color appears, and the contrast of the laminate becomes good.

[0034] <Resin fine particles> Resin fine particles refer to particulate resin. Some of the resin fine particles exhibit structural color due to regular arrangement. As the resin fine particles, resin fine particles made of a polymer of an ethylenically unsaturated monomer are preferred because they can easily produce monodisperse fine particles with a narrow particle size distribution that exhibit excellent structural color development. Resin fine particles made of an acrylic resin or a styrene-acrylic resin are more preferred because they can easily introduce reactive groups that can form crosslinks between adjacent particles in the pattern portion A and / or crosslinks between the pattern portion A and the adjacent coating layer and / or substrate.

[0035] Furthermore, the resin microparticles preferably have a core-shell structure in which the core and shell are water-insoluble polymers and the core (inner layer) and shell (outer layer) are incompatible with each other. The core functions to maintain the spherical shape, and the shell has fluidity and functions as a binding site. When a composition containing core-shell resin microparticles (hereinafter also referred to as a composition for pattern section A) is applied to a substrate, the core-shell resin microparticles are advected and accumulated to form a regularly arranged resin layer, and the shells of adjacent core-shell resin microparticles and the shells of the core-shell resin microparticles are easily bound to each other, and to the substrate layer or the primer layer described below, and the laminate exhibits excellent abrasion resistance.

[0036] When the resin particles constituting the resin layer are made of a polymer of an ethylenically unsaturated monomer, the desired resin particles can be obtained by emulsion polymerization of the ethylenically unsaturated monomer.

[0037] <Core-shell type resin microparticles> The method for producing core-shell type resin microparticles is not particularly limited, and can be exemplified by the method of polymerizing ethylenically unsaturated monomers in aqueous medium such as emulsion polymerization, or the phase inversion emulsification method of carrying out polymerization in non-aqueous system and then inverting the phase into aqueous phase while removing solvent, but it is preferable to use emulsion polymerization because it can achieve high molecular weight, low viscosity and high solid content concentration.In addition, in emulsion polymerization, it can also use either two-stage polymerization, in which the monomer composition is changed between the first stage and the second stage and is dropped, or multi-stage polymerization, in which the monomer composition is changed in three or more stages and is dropped.

[0038] The core-shell type resin particles can be prepared by the above-mentioned two-stage polymerization, specifically, by the following procedure.

[0039] (1) First, an aqueous medium and a surfactant are charged into a reaction vessel and the temperature is raised. Then, under a nitrogen atmosphere, a radical polymerization initiator is added while an emulsion of an ethylenically unsaturated monomer in the first stage, which will form the core, is added dropwise. After the reaction starts, the particles gradually grow to form core particles according to the amount added.

[0040] (2) Next, when the first-stage addition is completed and the heat generation has subsided, the second-stage addition of the emulsion of the ethylenically unsaturated monomer to form the shell is started. At this time, additional initiator may be added. The added second-stage ethylenically unsaturated monomer is initially distributed to the core particles, but as the polymerization proceeds, it precipitates as a polymer on the outer layer of the core particles, forming a shell layer.

[0041] <Ethylenically Unsaturated Monomer> Examples of the ethylenically unsaturated monomer include styrene, α-methylstyrene, o-methylstyrene, p-methylstyrene, m-methylstyrene, vinylnaphthalene, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, phenoxytetraethylene glycol (meth)acrylate, phenoxyhexaethylene glycol (meth)acrylate, phenoxyhexaethylene glycol (meth)acrylate, and phenyl (meth)acrylate. aromatic ethylenically unsaturated compounds such as acrylate, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, heptyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, lauryl (meth)acrylate, thiazolinone, linear or branched alkyl group-containing ethylenically unsaturated monomers such as tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, and behenyl (meth)acrylate; cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and dicyclopentanyl (meth)acrylate; Alicyclic alkyl group-containing ethylenically unsaturated monomers such as adamantyl (meth)acrylate; fluorinated alkyl group-containing ethylenically unsaturated monomers such as trifluoroethyl (meth)acrylate and heptadecafluorodecyl (meth)acrylate; carboxy group-containing ethylenically unsaturated monomers such as (anhydrous) maleic acid, fumaric acid, itaconic acid, citraconic acid, or alkyl or alkenyl monoesters thereof, succinic acid β-(meth)acryloxyethyl monoester, acrylic acid, methacrylic acid, crotonic acid, and cinnamic acid;Sulfo group-containing ethylenically unsaturated monomers such as sodium 2-acrylamido 2-methylpropanesulfonate, methallylsulfonic acid, methallylsulfonic acid, sodium methallylsulfonate, allylsulfonic acid, sodium allylsulfonate, ammonium allylsulfonate, and vinylsulfonic acid; (meth)acrylamide, N-methoxymethyl-(meth)acrylamide, N-ethoxymethyl-(meth)acrylamide, N-propoxymethyl-(meth)acrylamide, N-butoxymethyl-(meth)acrylamide, N-pentoxymethyl-(meth)acrylamide, N,N-di(methoxymethyl)acrylamide, N-ethoxymethyl-N-methoxymethylmethacrylamide, N,N-di(ethoxymethyl)acrylamide, N-ethoxymethyl-N-propoxymethylmethacrylamide, N,N-di(propoxymethyl)acrylamide, N-butoxymethyl-N-(propoxymethyl)methacrylamide, N,N-di(butoxymethyl) Amide group-containing ethylenically unsaturated monomers such as N-butyl (meth)acrylamide, N-butoxymethyl-N-(methoxymethyl)methacrylamide, N,N-di(pentoxymethyl)acrylamide, N-methoxymethyl-N-(pentoxymethyl)methacrylamide, N,N-dimethylaminopropylacrylamide, N,N-diethylaminopropylacrylamide, N,N-dimethylacrylamide, N,N-diethylacrylamide, and diacetone acrylamide; hydroxyl group-containing ethylenically unsaturated monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, glycerol mono(meth)acrylate, 4-hydroxyvinylbenzene, 1-ethynyl-1-cyclohexanol, and allyl alcohol; polyoxyethylene group-containing ethylenically unsaturated monomers such as methoxypolyethylene glycol (meth)acrylate and polyethylene glycol (meth)acrylate; amino group-containing ethylenically unsaturated monomers such as dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, methylethylaminoethyl (meth)acrylate, dimethylaminostyrene, and diethylaminostyrene;Epoxy group-containing ethylenically unsaturated monomers such as glycidyl (meth)acrylate and 3,4-epoxycyclohexyl (meth)acrylate; ketone group-containing ethylenically unsaturated monomers such as diacetone (meth)acrylamide, acetoacetoxy (meth)acrylate and 2-acetoacetoxyethyl (meth)acrylate; allyl (meth)acrylate, 1-methylallyl (meth)acrylate, 2-methylallyl (meth)acrylate, 1-butenyl (meth)acrylate, (meth)acrylate, 2-butenyl (meth)acrylate, 3-butenyl (meth)acrylate, 1,3-methyl-3-butenyl (meth)acrylate, 2-chloroallyl (meth)acrylate, 3-chloroallyl (meth)acrylate, o-allylphenyl (meth)acrylate, 2-(allyloxy)ethyl (meth)acrylate, allyl lactyl (meth)acrylate, citronellyl (meth)acrylate, geranyl (meth)acrylate, Ethylenically unsaturated monomers having two or more ethylenically unsaturated groups, such as rosinyl (meth)acrylate, cinnamyl (meth)acrylate, diallyl maleate, diaryl itaconic acid, vinyl (meth)acrylate, vinyl crotonate, vinyl oleate, vinyl linolenate, 2-(2'-vinyloxyethoxy)ethyl (meth)acrylate, ethylene glycol di(meth)acrylate, triethylene glycol (meth)acrylate, tetraethylene glycol (meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, 1,1,1-trishydroxymethylethane diacrylate, 1,1,1-trishydroxymethylethane triacrylate, 1,1,1-trishydroxymethylpropane triacrylate, divinylbenzene, divinyl adipate, diallyl isophthalate, diallyl phthalate, and diallyl maleate;Examples of such ethylenically unsaturated monomers include alkoxysilyl group-containing ethylenically unsaturated monomers such as γ-methacryloxypropyltrimethoxysilane, γ-methacryloxypropyltriethoxysilane, γ-methacryloxypropyltributoxysilane, γ-methacryloxypropylmethyldimethoxysilane, γ-methacryloxypropylmethyldiethoxysilane, γ-acryloxypropyltrimethoxysilane, γ-acryloxypropyltriethoxysilane, γ-acryloxypropylmethyldimethoxysilane, γ-methacryloxymethyltrimethoxysilane, γ-acryloxymethyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltributoxysilane, and vinylmethyldimethoxysilane; and methylol group-containing ethylenically unsaturated monomers such as N-methylol(meth)acrylamide, N,N-dimethylol(meth)acrylamide, and alkyl-etherified N-methylol(meth)acrylamide.

[0042] These monomers may be used alone or in combination of two or more.

[0043] <Average particle size> The average particle size of the resin microparticles may be, for example, 100 to 400 nm or 150 to 380 nm, but is preferably 160 to 350 nm, more preferably 190 to 320 nm, and even more preferably 220 to 280 nm. When the average particle size of the resin microparticles is in the range of 160 to 350 nm, contrast can be further improved. Note that the average particle size in the present disclosure can be measured by dynamic light scattering, and the peak of the obtained volume particle size distribution data (histogram) is taken as the average particle size.

[0044] Furthermore, the coefficient of variation (Cv value) of the average particle diameter of the resin microparticles is preferably 30% or less, more preferably 20% or less. When the coefficient of variation is 30% or less, the colored portion exhibits a vivid structural color, improving the contrast of the laminate. The coefficient of variation is a numerical value that represents the uniformity of the particle diameters and can be calculated using the following formula:

[0045] Formula: Coefficient of variation Cv value (%)=Standard deviation of particle size / Average particle size×100 (In the formula, the units of the standard deviation and the average particle size are the same)

[0046] <Glass transition point> When the resin microparticles are core-shell type resin microparticles, the glass transition point of the core is preferably 80°C or higher, more preferably 80 to 250°C. The glass transition point of the shell is preferably -20°C or higher, more preferably -20 to 100°C, and even more preferably -20 to 50°C. When the core has a glass transition point of 80°C or higher, deformation of the core shape due to external heat or force is suppressed. This allows the pattern portion A to maintain excellent color development during formation of the pattern portion B or during winding, resulting in good contrast of the laminate. When the shell has a glass transition point of -20°C or higher, the shell has appropriate fluidity and functions as a bonding site between particles, resulting in good abrasion resistance of the laminate. The glass transition point can be measured by DSC (differential scanning calorimeter).

[0047] <Particle Gaps> Pattern section A preferably has particle gaps, and air is preferably present in these particle gaps. The presence of air in the particle gaps increases the difference in refractive index between the particles and the particle gaps, resulting in excellent color development in the colored portion and good contrast in the laminate. In the present disclosure, if voids with a modest pore size of 10 to 200 nm are detected by the nitrogen adsorption method, it can be determined that the particle gaps in the resin layer are air. The modest pore size can be determined by the peak top of the nitrogen adsorption isotherm on the adsorption side, obtained by analysis based on the Barrett-Joyner-Halenda method (BJH method). In the BJH method, a reference t curve is calculated using a Harkins-Jura type equation and analyzed based on the volume frequency distribution. In the present disclosure, measurements were performed using a BELSORP-max II device manufactured by Microtrac-Bell Corporation.

[0048] <Additives> The pattern portion A may contain additives such as antifoaming agents, thickeners, surfactants, antiblocking agents, crosslinking agents, leveling agents, waxes, ultraviolet absorbers, and light stabilizers, as well as organic solvents such as alcohols, as needed.

[0049] <Formation of pattern portion A> The pattern portion A can be formed by applying a coating agent containing resin fine particles to a substrate and then drying it. The coating agent containing resin fine particles preferably contains resin fine particles and water. It is known that resin fine particle dispersions are regularly arranged as they dry, but at the same time, cracks are generated to a considerable extent.

[0050] <Method for producing a coating agent containing resin microparticles> A method for producing a coating agent containing resin microparticles for forming the pattern portion A will be described. The coating agent containing resin microparticles can be obtained, for example, by charging an aqueous dispersion of resin microparticles and any additives into a mixer equipped with a stirring blade, rotor, etc., and mixing and stirring them. The stirring speed is not particularly limited, and stirring can be carried out at 50 to 2000 rpm. In order to improve the handling and coatability of the coating agent containing resin microparticles, water and additives can also be added as appropriate.

[0051] <Pattern Section B> Pattern section B has a structure in which resin microparticles are irregularly arranged and does not exhibit structural color. In the present disclosure, "irregularly arranged resin microparticles" refers to the resin microparticles not being regularly arranged. It is sufficient that at least some of the resin microparticles remain, and includes cases in which the resin microparticles are partially dissolved and have an irregular shape, and cases in which the shells of the resin microparticles are fused together. The irregularly arranged resin microparticles result in a smooth coating film with fewer cracks than those that occur with a regular arrangement, thereby reducing unnecessary scattering. Therefore, the laminate of the present disclosure has excellent contrast, gloss, and abrasion resistance. The resin microparticles can be the same as the <Resin Microparticles> described in the above <Pattern Section A>. For example, compared to the regularly arranged resin microparticles of pattern section A, pattern section B may be in a state in which the resin microparticles are partially or entirely dissolved and have an irregular shape, a state in which the shells of the resin microparticles are partially or entirely fused together, or a combination thereof. In another example, in contrast to the state in which the resin particles in pattern portion A are regularly arranged, the resin particles in pattern portion B may be dispersed unevenly, resulting in a biased distribution of the resin particles.

[0052] It is preferable that pattern portion B contains amorphous resin fine particles. Pattern portion B can be formed by applying a coating agent that does not contain resin fine particles, which will be described later, to a part of pattern portion A. In this case, it is preferable that the resin fine particles contained in pattern portion A are partially dissolved and partially converted into amorphous resin fine particles.

[0053] The film thickness of pattern portion B is preferably 5 to 30 μm, more preferably 7 to 20 μm, and even more preferably 8 to 15 μm. When the film thickness of pattern portion A is taken as 100%, the film thickness of pattern portion B is preferably 80 to 120%, or preferably 90 to 110%, and even more preferably ±5%. By eliminating the difference in film thickness between pattern portion A and pattern portion B, the occurrence of wrinkles in the film can be prevented, and the contrast and gloss can be further improved.

[0054] When the diffuse reflectance spectrum of the pattern portion B is measured at an incident angle of 5°, it is preferable that the pattern portion B does not exhibit a reflection peak having a half-width of less than 100 nm and a reflected light intensity of 5% or more in the wavelength range of 380 nm to 2000 nm. When the pattern portion B does not exhibit the above optical characteristics, the contrast of the laminate becomes good.

[0055] <Other Resins> The pattern portion B of the present disclosure may contain resins other than the above-described resin particles, such as acrylic resins, urethane resins, polyolefin resins, polyester resins, and composite resins obtained by combining these resins, and may contain one or more of these.

[0056] <Additives> The pattern portion B of the present disclosure may contain a colorant, an ultraviolet absorber, or a light stabilizer for adjusting the color tone of the structural color or for protecting the structural color. When the pattern portion B contains an ethylenically unsaturated monomer, it may contain a photopolymerization initiator for the purpose of curing the coating film.

[0057] <Formation of Pattern Section B> Pattern section B can be formed by applying a coating agent that does not contain resin microparticles to a portion of pattern section A. In this case, some or all of the resin microparticles in pattern section A melt or fuse by the coating agent, changing pattern section A to pattern section B, thereby forming pattern section B. In another example, pattern section B can be formed by applying a coating agent that contains a thickener or the like together with resin microparticles to a portion of pattern section A. In this case, the resin microparticles applied by the coating agent are unevenly distributed by the thickener or the like, thereby forming pattern section B. In yet another example, pattern section B can be formed by applying a coating agent that contains a resin and a non-aqueous low-molecular-weight component to a portion of pattern section A. In this case, some or all of the resin microparticles in pattern section A melt or fuse by the non-aqueous low-molecular-weight component, changing pattern section A to pattern section B, thereby forming pattern section B. Alternatively, the resin can remain on pattern section B to form a coating layer.

[0058] <Coating agent not containing resin microparticles> The coating agent not containing resin microparticles preferably contains a non-aqueous low-molecular component. The coating agent not containing resin microparticles preferably further contains a non-aqueous resin described below. When the coating agent not containing resin microparticles contains a non-aqueous resin, by applying this onto the pattern portion A, the formation of the pattern portion B and the formation of the coating layer C described below can be performed simultaneously.

[0059] <Non-aqueous low molecular weight component> The non-aqueous low molecular weight component contained in the coating agent that does not contain resin microparticles is not particularly limited as long as it can disrupt the shape and regular array structure of the resin microparticles. Examples of such non-aqueous low molecular weight components include organic solvents such as toluene, xylene, methylcyclohexane, ethyl acetate, normal propyl acetate, butyl acetate, isopropanol, butanol, methyl ethyl ketone, and methyl isobutyl ketone, as well as the ethylenically unsaturated monomers described in the above section <Ethylenically unsaturated monomer>.

[0060] <Thickener> Examples of thickeners include sodium polycarboxylate, modified polyacrylic acid-based thickeners, polyether-based thickeners, urethane-modified polyether-based thickeners, and water-soluble cellulose ether-based thickeners, with modified polyacrylic acid-based thickeners being more preferred. When a thickener is contained in a coating agent, the resin fine particles cannot be dispersed evenly and are distributed irregularly, resulting in no structural color.

[0061] <Coating Layer> The laminate of the present disclosure preferably further has a coating layer on the pattern portion A and / or the pattern portion B. When the laminate has a coating layer, scattering caused by resin fine particles and cracks in the pattern portion A and / or the pattern portion B is suppressed, and the contrast and gloss of the laminate are further improved.

[0062] In the present disclosure, the coating layer located on the pattern portion A is referred to as coating layer D, and the coating layer located on the pattern portion B is referred to as coating layer C.

[0063] The laminate of the present disclosure preferably has coating layer C and / or coating layer D, more preferably has coating layer C, and particularly preferably has coating layer C and coating layer D.

[0064] The thickness of the coating layer is preferably 0.1 to 10 μm. When the thickness of the coating layer is 0.1 μm or more, scattering caused by resin fine particles and cracks in pattern portion A and / or pattern portion B is suppressed, thereby further improving the contrast and gloss of the laminate. Furthermore, when the thickness of the coating layer is 10 μm or less, the maximum film thickness difference within the plane of the laminate is kept small, improving the winding properties of the laminate.

[0065] <Colorant> The coating layer preferably contains a colorant. By including a colorant in the coating layer, scattered light unrelated to the structural color can be reduced when the laminate is observed from the uncoated side in a reverse printing configuration, thereby improving the contrast of the laminate. The type of colorant is not particularly limited, and examples include pigments and dyes, with pigments being preferred. The pigments that can be used in the present disclosure are not particularly limited, and various inorganic and organic pigments that can generally be used in printing inks and paints can be suitably used. Examples of inorganic pigments include colored pigments such as titanium oxide, red iron oxide, Prussian blue, ultramarine blue, carbon black, and graphite, as well as extender pigments such as calcium carbonate, kaolin, clay, barium sulfate, aluminum hydroxide, and talc. Suitable organic pigments include soluble azo pigments, insoluble azo pigments, azo lake pigments, condensed azo pigments, copper phthalocyanine pigments, and condensed polycyclic pigments. However, the pigments are not limited to these, and any pigment listed by its generic name in the Color Index can be used as appropriate.

[0066] <Additives> The coating layer may contain additives such as antifoaming agents, thickeners, surfactants, antiblocking agents, crosslinking agents, leveling agents, waxes, ultraviolet absorbers, and light stabilizers, as needed.

[0067] <Coating Layer C> By positioning the coating layer C on the pattern portion B, fading of the structural color of the pattern portion B is further accelerated and scattering is reduced, thereby improving the contrast and gloss of the laminate. The film thickness of the coating layer C is preferably 0.3 to 25 μm, more preferably 0.8 to 20 μm, and even more preferably 1 to 18 μm. By setting the film thickness of the coating layer C to 10 μm or less, 5 μm or less, or 3 μm or less, the maximum film thickness difference within the plane of the laminate can be kept small, and the winding ability of the laminate can be further improved.

[0068] The coating layer C preferably contains a resin, and in particular, preferably contains a non-aqueous resin. Furthermore, as described above, the coating layer C preferably further contains a colorant. When the coating layer C contains a colorant, the content thereof in the coating layer C is preferably 0.1 to 50 mass %. The coating layer C may be a single layer or a multilayer of two or more layers. When the coating layer C is a multilayer, it may contain a non-aqueous resin layer and an aqueous resin layer. In this case, it is more preferable that the pattern portion B, the non-aqueous resin layer, and the aqueous resin layer are laminated in this order. The aqueous resin layer may be the same as the coating layer D described below.

[0069] <Non-aqueous Resin> The non-aqueous resin that can be contained in the coating part C refers to a resin that can be dispersed or dissolved in an organic solvent, and does not include hydrophilic resins. The non-aqueous resin may contain at least one resin selected from the group consisting of, for example, acrylic resin, styrene-acrylic resin, urethane resin, vinyl chloride resin, vinyl chloride-vinyl acetate resin, vinyl chloride-acrylic resin, polyolefin resin, polyester resin, soluble nitrocellulose, polyamide resin, and composite resins obtained by combining these resins.

[0070] The non-aqueous resin preferably contains an acrylic resin, a styrene-acrylic resin, or a urethane resin, and more preferably is a styrene-acrylic resin or a urethane resin, since it has a high affinity with the resin particles and improves the abrasion resistance of the laminate.

[0071] <Formation of Coating Layer C> Coating layer C can be formed by applying a coating agent containing a resin onto pattern portion A or pattern portion B, followed by drying. The coating agent is preferably a coating agent containing a non-aqueous resin. Alternatively, coating layer C can be formed by applying a coating agent containing a UV monomer onto pattern portion A or pattern portion B, followed by UV irradiation.

[0072] In addition, by applying a coating agent containing resin but not resin microparticles onto pattern portion A and then drying it, pattern portion B can be formed and coating layer C can be formed on pattern portion B simultaneously.

[0073] <Coating agent containing non-aqueous resin> The coating agent containing a non-aqueous resin preferably contains a non-aqueous resin and a non-aqueous low-molecular-weight component, and more preferably further contains a colorant. It may also contain additives that may be contained in the coating layer as appropriate. The non-aqueous low-molecular-weight component may be the same as that described in the above-mentioned <Pattern section B>.

[0074] <Method for producing a coating agent containing a non-aqueous resin> A coating agent containing a non-aqueous resin can be produced, for example, by dispersing a pigment in a non-aqueous low-molecular-weight component using a disperser with a non-aqueous resin or the like, and then mixing the resulting pigment dispersion with the non-aqueous resin, various additives, and the non-aqueous low-molecular-weight component. Commonly used dispersers, such as a roller mill, ball mill, pebble mill, attritor, and sand mill, can be used. The particle size distribution of the pigment in the pigment dispersion can be adjusted by appropriately adjusting the size of the grinding media in the disperser, the filling rate of the grinding media, the dispersion treatment time, the discharge speed of the pigment dispersion, the viscosity of the pigment dispersion, and the like. The viscosity of the coating agent containing a non-aqueous resin at 25°C is preferably 10 mPa·s or more from the viewpoint of preventing pigment sedimentation and adequate dispersion, and 300 mPa·s or less from the viewpoint of workability and efficiency during ink production and printing.

[0075] <Coating Layer D> By positioning the coating layer D on the pattern portion A, the excellent structural color of the pattern portion A is maintained, and the contrast and gloss of the laminate are improved. The film thickness of the coating layer D is preferably 0.2 to 12 μm, more preferably 0.5 to 9 μm, and even more preferably 1 to 5 μm.

[0076] The coating layer D preferably contains a resin, and more preferably contains an aqueous resin. As described above, the coating layer D also preferably contains a colorant.

[0077] <Formation of Coating Layer D> The coating layer D can be formed by applying a coating agent containing a resin onto the pattern portion A and then drying the coating agent. The coating agent is preferably a coating agent containing an aqueous resin.

[0078] <Coating agent containing aqueous resin> The coating agent containing aqueous resin preferably contains an aqueous resin and an aqueous medium, and more preferably further contains a colorant. It may also contain additives that may be contained in the coating layer as appropriate. The aqueous resin contained in the coating agent containing aqueous resin refers to a resin that can be dispersed or dissolved in an aqueous medium. The aqueous resin preferably contains at least one resin selected from the group consisting of, for example, acrylic resin, urethane resin, polyolefin resin, polyester resin, and composite resins obtained by combining these resins. It is preferable that the aqueous resin contains an acrylic resin, a styrene-acrylic resin, or a urethane resin, since it has a high affinity with resin microparticles and improves the abrasion resistance of the laminate.

[0079] <Aqueous Medium> The main component of the aqueous medium is preferably water, but in addition to water, a hydrophilic organic solvent can be used. Specifically, depending on the printing conditions (speed, plate depth, design, drying temperature), an alcohol-based organic solvent, a glycol-based organic solvent, etc. can be added.

[0080] In the present disclosure, "the main component is water" means that the water content is the largest in the aqueous medium. Furthermore, "hydrophilic organic solvent" refers to a solvent that is liquid at 25°C and has a solubility in water at 25°C of 1% by mass or more.

[0081] <Method for producing a coating agent containing an aqueous resin> A coating agent containing an aqueous resin can be produced, for example, by dispersing a pigment in an aqueous medium using a disperser with an aqueous resin or the like, and then mixing the resulting pigment dispersion with the aqueous resin, various additives, an aqueous medium, and the like. Commonly used dispersers, such as a roller mill, ball mill, pebble mill, attritor, and sand mill, can be used. The particle size distribution of the pigment in the pigment dispersion can be adjusted by appropriately adjusting the size of the grinding media in the disperser, the filling rate of the grinding media, the dispersion treatment time, the discharge speed of the pigment dispersion, the viscosity of the pigment dispersion, and the like. The viscosity of the coating agent containing an aqueous resin at 25°C is preferably 10 mPa·s or more from the viewpoint of preventing pigment sedimentation and adequate dispersion, and 300 mPa·s or less from the viewpoint of workability and efficiency during ink production and printing.

[0082] <Substrate> The substrate is not particularly limited and can be appropriately selected depending on the application. Examples include thermoplastic resin substrates such as polyvinyl chloride sheets, polyethylene terephthalate (PET) films, polypropylene films, polyethylene films, nylon films, polystyrene films, and polyvinyl alcohol films; metal substrates such as aluminum foil; glass substrates, paper substrates such as coated paper; and cloth substrates. The substrate may have a smooth or uneven coating surface. The substrate may be transparent, translucent, or opaque, and may be a substrate that has been pre-colored, for example, black, to make the color of the pattern portion A more distinct. These substrates may be used alone or as a laminate composed of two or more layers.

[0083] The thickness of the substrate is not particularly limited and can be selected appropriately in the range of usually 5 to 500 μm.

[0084] <Primer Layer> The laminate of the present disclosure preferably has a primer layer to further improve the fixation of the pattern portion A and the pattern portion B on the substrate. The primer layer is located between the substrate and the pattern portion A and the pattern portion B, and can be formed by applying a primer coating agent onto the substrate before the formation of the pattern portion A.

[0085] The thickness of the primer layer is preferably 0.5 to 30 μm, more preferably 0.8 to 15 μm, and particularly preferably 1 to 5 μm.

[0086] From the viewpoint of suppressing the influence on the pattern portion A and the pattern portion B, the primer layer preferably has a low content of unreacted components and residual solvents, and is preferably formed from an aqueous resin.

[0087] The aqueous resin forming the primer layer is not particularly limited and can be appropriately selected depending on the type of substrate and pattern portion A. Preferably, it contains at least one selected from the group consisting of acrylic resins, urethane resins, polyolefin resins, polyester resins, and composite resins obtained by combining these resins. Among these, from the viewpoints of excellent adhesion to the substrate and pattern portion A, and excellent water resistance, solvent resistance, and transparency of the primer layer, it preferably contains an acrylic resin and / or a urethane resin, more preferably contains an acrylic resin, and even more preferably contains an acrylic resin containing styrene as a structural unit (hereinafter referred to as a styrene-acrylic resin). The use of a styrene-acrylic resin is preferred because it provides excellent adhesion to the substrate and pattern portion A, excellent substrate conformability and water resistance of the primer layer, and good substrate conformability, abrasion resistance, and water resistance of the laminate. These resins may be used alone or in combination of two or more.

[0088] <Primer Coating Agent> The method for forming the primer layer is not particularly limited. For example, the primer layer can be formed by applying a primer coating agent containing an aqueous resin and an aqueous medium that form the primer layer onto a substrate and drying it as necessary.

[0089] The primer coating agent may contain various additives such as hydrophilic solvents, achromatic black fine particles, photothermal conversion agents, crosslinking agents, etc., for the purpose of improving the coatability, contrast, gloss, and winding properties of the laminate, as long as they do not adversely affect the physical properties of the laminate.

[0090] <Steps on the Coated Surface of the Laminate> The step (maximum film thickness difference) on the coated surface of the laminate of the present disclosure is preferably 10 μm or less, preferably 5 μm or less, and more preferably 0 to 3 μm. Having a step of 10 μm or less prevents wrinkles in the film due to unevenness in the coating film when the laminate is wound up, resulting in good contrast and gloss. For example, by producing a laminate by changing pattern portion A to pattern portion B, the surface of the laminate is flattened, making it possible to further reduce these steps. In the present disclosure, the maximum film thickness difference on the coated surface of the laminate refers to the difference in film thickness between pattern portion A and pattern portion B.

[0091] <Method for manufacturing laminate> The method for manufacturing a laminate of the present disclosure includes step 1 of applying a coating agent containing resin microparticles onto a substrate or a primer layer to form a pattern portion A that exhibits structural color due to the regular arrangement of the resin microparticles, and step 2 of applying a coating agent that does not contain resin microparticles to a part of pattern portion A to change pattern portion A into pattern portion B that does not exhibit structural color.

[0092] In step 2, it is preferable that the regular arrangement of resin microparticles in pattern portion A formed in step 1 is disrupted by application of a coating agent that does not contain resin microparticles, and pattern portion B in which resin microparticles are present in an irregular manner is formed.

[0093] In step 2, it is preferable that the resin particles in the pattern portion A formed in step 1 are partially dissolved by the application of the coating agent containing no resin particles, and some of them are converted into amorphous resin particles.

[0094] In step 2, it is preferable to use a coating agent containing a non-aqueous resin as the coating agent without resin particles, so that the pattern portion B and the coating layer C are formed simultaneously.

[0095] Furthermore, the method for producing a laminate according to the present disclosure preferably further includes a step of forming a coating layer D by applying a coating agent containing an aqueous resin onto the pattern portion A.

[0096] <Coating Method> The coating method for various coating agents is not particularly limited, and can be formed using a known printing method. Examples of the printing method include plateless printing methods such as inkjet printing, spraying, dipping, slot die printing, and spin coating; and plate printing methods such as offset gravure coater, gravure coater, doctor coater, kiss coater, bar coater, blade coater, flexo coater, and roll coater.

[0097] The coating agent containing resin fine particles is preferably applied by a spray method, a dipping method, a slot die method, a spin coating method, a gravure coater, a doctor coater, a kiss coater, a bar coater, a blade coater, or a roll coater. By using any of the above methods for applying the coating agent containing resin fine particles, the color development of the pattern portion A is excellent and the contrast of the laminate is improved.

[0098] The coating speed of the coating agent containing resin fine particles is preferably 0.1 to 100 m / min. When the coating speed is 100 m / min or less, the fine particles form a precise regular arrangement, resulting in excellent color development of the pattern portion A.

[0099] The coating method for coating agents that do not contain resin particles is preferably an inkjet method, a spray method, an offset gravure coater, a gravure coater, or a flexo coater, because these methods facilitate pattern formation.

[0100] Furthermore, the coating speed of the coating agent that does not contain resin fine particles is preferably 20 m / min or more. By using a coating speed of 20 m / min or more, it is possible to form a clear pattern portion B and the productivity of the laminate is also improved.

[0101] In the present disclosure, the thickness of each layer is measured by observing the cross section of the laminate using a scanning electron microscope. The measurement locations are not particularly limited, but the thickness is measured at multiple locations for each layer to be measured, for example, 10 locations, and the arithmetic average value is used.

[0102] The present invention will be described below with reference to examples, but is not limited to these. In the examples and comparative examples, "parts" and "%" mean "parts by mass" and "% by mass" unless otherwise specified.

[0103] <Average particle size, Cv value> The average particle size was measured by diluting the fine particle dispersion 500 times with water, measuring about 5 ml of the diluted solution by dynamic light scattering measurement (measuring device manufactured by Nanotrac UPA Co., Ltd., Microtrac Bell Co., Ltd.), and the peak of the obtained volume particle size distribution data (histogram) was taken as the average particle size. In addition, the coefficient of variation Cv value, which represents the uniformity of the particle size, was calculated by the following formula.

[0104] Formula: Cv value (%) = standard deviation of particle diameter / average particle diameter × 100 (In the formula, the units of the standard deviation and the average particle diameter are the same.)

[0105] <Glass transition point> The glass transition point was measured by DSC (differential scanning calorimeter manufactured by TA Instruments Co., Ltd.) Specifically, about 2 mg of a sample obtained by drying a resin fine particle dispersion was weighed on an aluminum pan, the aluminum pan was set in a DSC measurement holder, and the endothermic peak in a chart showing a baseline shift (inflection point) toward the endothermic side of a DSC curve obtained under a temperature increase condition of 5°C / min was read to obtain the glass transition point.

[0106] <Acid Value> The acid value is the number of milligrams of potassium hydroxide required to neutralize the free fatty acids, resin acids, etc. contained in 1 g of a sample, and was measured by the method described in JIS K 0070.

[0107] <Amine Value> The amine value is the amount of potassium hydroxide (mg) equivalent to the amount of hydrochloric acid required to neutralize the amino groups contained in 1 g of sample, and was measured in accordance with JIS K 0070. 0.5 to 2 g of sample was precisely weighed (sample solids: S g), and 50 mL of a 60 / 40 (mass ratio) mixed solution of methanol and methyl ethyl ketone was added to the precisely weighed sample for dissolution. Bromophenol blue was added as an indicator to the resulting solution, and the resulting solution was titrated with a 0.2 mol / L ethanolic hydrochloric acid solution (titer: f). The point at which the color of the solution changed from green to yellow was defined as the endpoint, and the titration volume (A mL) at this point was used to calculate the amine value according to the following formula:

[0108] (Formula) Amine value = (A × f × 0.2 × 56.108) / S [mg KOH / g]

[0109] <Weight-average molecular weight> The weight-average molecular weight was determined by measuring the molecular weight distribution using a gel permeation chromatography (GPC) device (HLC-8220 manufactured by Tosoh Corporation) and calculating the molecular weight converted using polystyrene as a standard substance. The measurement conditions are shown below.

[0110] Columns: The following columns were used in series.

[0111] TSKgel Super AW2500 manufactured by Tosoh Corporation TSKgel Super AW3000 manufactured by Tosoh Corporation TSKgel Super AW4000 manufactured by Tosoh Corporation TSKgelguard column Super AWH manufactured by Tosoh Corporation Detector: RI (differential refractometer) Measurement conditions: Column temperature 40°C Eluent: tetrahydrofuran Flow rate: 1.0 mL / min

[0112] <Shape and Arrangement of Resin Particles> The shape and arrangement of the resin particles were measured by observing the cross section of the laminate with a scanning electron microscope (JSM-7800F manufactured by JEOL Ltd.).

[0113] <Method for measuring the film thickness of each layer> In measuring the film thickness of each layer, two laminate samples were prepared, and the cross sections were observed using a scanning electron microscope (JEOL Ltd., JSM-7800F) at a measurement magnification of 2000 times, and measurements were taken at five locations on each layer to be measured for each laminate sample, and the arithmetic mean value of the measurement results at a total of 10 locations was taken as the film thickness.

[0114] <Method for measuring maximum film thickness difference> In the method for measuring the maximum film thickness difference, two laminate samples were prepared, and the measurement magnification of the cross section was set to 2000 times using a scanning electron microscope (JEOL JSM-7800F), and the film thickness difference between pattern portion A and the adjacent pattern portion B of the layer was measured at five locations for each laminate sample, and the maximum value of the measurement results at a total of 10 locations was taken as the maximum film thickness difference.

[0115] <Measurement of half-value width, reflection wavelength, and reflected light intensity> The diffuse reflectance spectrum of the laminate was measured in the wavelength range of 350 to 2000 nm using an ultraviolet-visible-near-infrared spectrophotometer (V-770D manufactured by JASCO Corporation, integrating sphere unit ISN-923). The reflectance at each wavelength is the relative reflectance measured using a standard white plate with known reflectance (SRS-99-010 manufactured by Labsphere) as a reference.

[0116] The half-width, reflection wavelength, and reflection intensity of the reflection peak with the highest reflection intensity in the obtained reflection spectrum were read.

[0117] <Production of Resin Particles> [Production Example 1] Production of Core-Shell Resin Particles 99.0 parts of styrene, 1.0 part of acrylic acid, 4.0 parts of a 25% aqueous solution of Aqualon AR-10 (manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd., an anionic reactive surfactant (polyoxyethylene styrenated phenyl ether sulfates)) (solids content: 1.0 part), and 39.0 parts of ion-exchanged water were mixed and stirred to prepare a first-stage emulsion of ethylenically unsaturated monomers. 95.0 parts of ion-exchanged water and 1.5% of the first-stage emulsion were added to a reaction vessel equipped with a stirrer, thermometer, dropping funnel, and reflux condenser. The internal temperature of the reaction vessel was raised to 70°C and thoroughly purged with nitrogen, and then 6.0 parts of a 2.5% aqueous solution of potassium persulfate (solids content: 0.15 parts) was added as an initiator to initiate polymerization. The internal temperature was raised to 80° C. and, while maintaining the temperature, the remainder of the emulsion and 4.2 parts of a 2.5% aqueous solution of potassium persulfate (solid content: 0.11 parts) were added dropwise over 2 hours to react them, synthesizing core particles.

[0118] Next, 27.6 parts of styrene, 13.2 parts of n-butyl acrylate, 2.2 parts of methacrylic acid, 1.7 parts of a 25% aqueous solution of Aqualon AR-10 (solids content: 0.4 parts), and 16.7 parts of ion-exchanged water were mixed and stirred to prepare a second-stage emulsion of ethylenically unsaturated monomers. 20 minutes after the completion of the first-stage dropwise addition, the second-stage emulsion was started to be added dropwise. While maintaining the internal temperature at 80°C, the second-stage emulsion and 1.6 parts of a 2.5% aqueous solution of potassium persulfate (solids content: 0.04 parts) were added dropwise over 2 hours to proceed with the reaction, and an aqueous dispersion of core-shell type resin microparticles was obtained.

[0119] After the reaction, water was added to adjust the solid content to 45.0%. 3 The core-shell resin microparticles were neutralized by adding 1.7 parts of aqueous ammonia (aq). The amount of aqueous ammonia was equivalent to the amount required to neutralize all carboxyl groups contained in the shell (hereinafter, referred to as 1 equivalent). The average particle size of the resulting microparticles was 258 nm, the Cv value was 12.9%, the Tg of the core was 100.1°C, and the Tg of the shell was 51.8°C.

[0120] [Production Examples 2 to 5] Production of Core-Shell Resin Microparticles In Production Examples 2 to 5, the amount of the first-stage emulsion charged to the reaction vessel was changed from 1.5% in Production Example 1 to 0.9%, 1.0%, 3.0%, and 3.3%, respectively. Otherwise, the same procedure as in Production Example 1 was used to obtain aqueous dispersions of core-shell resin microparticles, as shown in Table 1. The reaction vessel was charged with water at a concentration of 67% relative to the total amount of ethylenically unsaturated monomer. The ethylenically unsaturated monomer emulsion was prepared by adding water so that the ethylenically unsaturated monomer concentration in the emulsion was 69% and the surfactant concentration was 0.69%. The proportions of the 2.5% aqueous potassium persulfate solution at the start of the reaction, during the dropwise addition of the first-stage emulsion, and during the dropwise addition of the second-stage emulsion were the same as in Production Example 1. Furthermore, 1 equivalent of aqueous ammonia relative to the carboxyl groups contained in the shell was added to neutralize the core-shell resin microparticles.

[0121]

[0122] [Production Example 6] Production of single-structure resin microparticles 99.0 parts of styrene, 1.0 part of methacrylic acid, 3.6 parts of a 25% aqueous solution of Aqualon AR-10 (solid content 0.9 parts), and 40.4 parts of ion-exchanged water were mixed and stirred in advance to prepare an emulsion of an ethylenically unsaturated monomer.

[0123] A reaction vessel equipped with a stirrer, thermometer, dropping funnel, and reflux condenser was charged with 68.9 parts of ion-exchanged water and 3% of the emulsion. The internal temperature was raised to 80 ° C. and thoroughly purged with nitrogen. 6.0 parts of a 2.5% aqueous solution of potassium persulfate (0.15 parts solids) was then added as an initiator to initiate emulsion polymerization. While maintaining the internal temperature at 80 ° C., the remainder of the emulsion and 6.0 parts of a 2.5% aqueous solution of potassium persulfate (0.15 parts solids) were added dropwise over 3 hours, and the reaction was continued for another 4 hours to obtain an aqueous dispersion of styrene-acrylic resin. After completion of the reaction, 1 equivalent of aqueous ammonia was added relative to the carboxyl groups contained in the resin microparticles to neutralize them, and the solids content of the aqueous dispersion was adjusted to 45.0% with ion-exchanged water. The average particle diameter of the resulting microparticles was 251 nm, the Cv value was 13.4%, and the Tg was 116.1 ° C.

[0124] [Production Example 7] Production of resin microparticles 40.2 parts of styrene, 57.8 parts of n-butyl acrylate, 2.0 parts of methacrylic acid, 4.0 parts of a 25% aqueous solution of Aqualon AR-10 (solid content: 1.0 part), and 40.4 parts of ion-exchanged water were mixed and stirred in advance to prepare an emulsion of an ethylenically unsaturated monomer.

[0125] A reaction vessel equipped with a stirrer, thermometer, dropping funnel, and reflux condenser was charged with 68.9 parts of ion-exchanged water and 3% of the emulsion. The internal temperature was raised to 80 ° C. and thoroughly purged with nitrogen. 6.0 parts of a 2.5% aqueous solution of potassium persulfate (0.15 parts solids) was then added as an initiator to initiate emulsion polymerization. While maintaining the internal temperature at 80 ° C., the remainder of the emulsion and 6.0 parts of a 2.5% aqueous solution of potassium persulfate (0.15 parts solids) were added dropwise over 3 hours, and the reaction was continued for another 4 hours to obtain an aqueous dispersion of styrene-acrylic resin. After completion of the reaction, 1 equivalent of aqueous ammonia was added relative to the carboxyl groups contained in the resin microparticles to neutralize them, and the solids content of the aqueous dispersion was adjusted to 45.0% with ion-exchanged water. The average particle diameter of the resulting microparticles was 225 nm, the Cv value was 13.9%, and the Tg was 7.4 ° C.

[0126] [Production Example 8] Production of urethane resin 1 100 parts of a polyester polyol having a number average molecular weight of 2,000, which is a condensate of 3-methyl-1,5-pentanediol and sebacic acid, 1 part of 1,4-butanediol, 28.5 parts of isophorone diisocyanate, and 32.1 parts of ethyl acetate were mixed and reacted in a nitrogen atmosphere at 90°C for 5 hours to obtain a urethane prepolymer having a terminal isocyanate group.

[0127] Next, 11.0 parts of isophoronediamine, 1.0 parts of N-(2-aminoethyl)ethanolamine, 1.0 parts of dibutylamine, and 298.1 parts of mixed solvent 1 (ethyl acetate / isopropanol = 70 / 30 (mass ratio)) were stirred and mixed, and the resulting isocyanate-terminated urethane prepolymer was gradually added at 40 ° C. The mixture was allowed to react at 80 ° C. for 1 hour, yielding a solution of urethane resin 1 with a solids content of 30 mass %, an amine value of 6.5 mg KOH / g, a hydroxyl value of 3.8 mg KOH / g, and a weight average molecular weight of 50,000. The chlorine content of urethane resin 1 was 0 mass %.

[0128] <Coating agent containing resin microparticles> [Production Example 9] 1.0 part of Surfynol 420 (manufactured by Nisshin Chemical Industry Co., Ltd., an acetylene-based nonionic surfactant) as a surfactant was added to 100.0 parts of the aqueous dispersion of the core-shell type resin microparticles of Production Example 1 and stirred to prepare a coating agent containing resin microparticles.

[0129] [Production Examples 10 to 15] Coating compositions containing resin fine particles were prepared in the same manner as in Production Example 9, except that the blending compositions were changed to those shown in Table 2.

[0130]

[0131] <Primer coating agent> [Production Example 16] A primer coating agent was prepared by adding 1.0 part of Surfynol 420 (an acetylene-based nonionic surfactant, manufactured by Nisshin Chemical Industry Co., Ltd.) as a surfactant to 100.0 parts of the aqueous dispersion of resin microparticles of Production Example 7 and stirring the mixture.

[0132] <Coating agent containing non-aqueous resin> [Production Example 17] 190.0 parts of methyl ethyl ketone as a non-aqueous low-molecular component was added to 210.0 parts of 7550MA (solid content 47.5%, ethyl acetate / IPA solution, oil-based styrene-acrylic resin) manufactured by Taisei Fine Chemical Co., Ltd., and the mixture was stirred to prepare a coating agent containing a non-aqueous resin.

[0133] [Production Examples 18 to 27] Coating agents containing non-aqueous resins were prepared in the same manner as in Production Example 17, except that the blending compositions were changed to those shown in Table 3.

[0134]

[0135] <Coating agent containing aqueous resin> [Production Example 28] To 260.0 parts of JONCRYL PDX7326 manufactured by BASF, 1.0 part of Surfynol 420 as a surfactant, 5.0 parts of Mitsubishi Carbon Black #40 as a colorant, and 240.0 parts of water were added to adjust the solids content to 20%, and the mixture was stirred to prepare a coating agent containing an aqueous resin.

[0136] [Production Examples 29 to 32] Coating agents containing aqueous resins were prepared in the same manner as in Production Example 28, except that the blending compositions were changed to those shown in Table 4.

[0137]

[0138] The abbreviations in Tables 2 to 4 are as follows:

[0139] Styrene acrylic 1: 7550MA manufactured by Taisei Fine Chemical (solid content 47.5%, ethyl acetate / IPA solution, oil-based styrene acrylic resin) Urethane 1: urethane resin 1 manufactured in Production Example 8 PVC acrylic: BINNOL E15 / 40A manufactured by Tomoe Engineering (oil-based PVC-acrylic resin) Polyamide: Vegichem Green 725 manufactured by Tsuno Foods Industries (solid content 25%, ethyl acetate / IPA=1 / 1 solution, oil-based polyamide resin) Nitrocellulose: NC TR2 manufactured by TNC INDUSTRIAL (solid content 25%, ethyl acetate / IPA=1 / 1 solution, oil-based nitrocellulose resin) Polyester 1: Vylon 200 manufactured by Toyobo (oil-based polyester resin) Styrene acrylic 2: JONCRYL PDX7326 manufactured by BASF (solid content 38.5%, aqueous styrene acrylic resin) Urethane 2: Superflex 210 (35% solids, aqueous polyurethane resin) manufactured by Daiichi Kogyo Seiyaku Co., Ltd. Polyolefin: Auroren AE-301 (30% solids, aqueous polyolefin resin) manufactured by Nippon Paper Industries Co., Ltd. Polyester 2: Pluscoat Z-221 (20% solids, aqueous polyester resin) manufactured by Goo Chemical Co., Ltd. MEK: methyl ethyl ketone EA: ethyl acetate MCH: methylcyclohexane IPA: isopropanol Surfynol 420: acetylene-based nonionic surfactant manufactured by Nissin Chemical Industry Co., Ltd. SN Thickener 617: acrylic thickener manufactured by San Nopco Ltd. Mitsubishi Carbon Black #40: carbon black manufactured by Mitsubishi Chemical Corporation TMP-A: Light Acrylate TMP-A (trimethylolpropane triacrylate) manufactured by Kyoeisha Chemical Co., Ltd. Omnirad 1173: Omnirad 1173 manufactured by IGM Resins (2-hydroxy-2-methyl-1-phenylpropanone) <Production of Laminate> [Example 1] A primer coating agent shown in Table 5 was applied to the corona-treated surface of Toyobo Ester Film E5100 using a bar coater to a thickness of 3.0 μm after drying, and then dried at 70° C. for 1 minute to form a primer layer. Next, a coating agent containing resin fine particles shown in Table 5 was applied to the primer layer using a bar coater to a thickness of 10.0 μm after drying, and then dried at 50° C. for 1 minute to form pattern portion A.Furthermore, a coating agent containing a non-aqueous resin was applied to a portion of the pattern portion A by gravure printing using a selected plate so that the thickness after drying would be 1.5 μm, thereby forming a pattern portion B and a coating layer C. Next, a coating agent containing an aqueous resin was applied to the pattern portion A and the coating layer C using a selected bar coater so that the thickness after drying would be 1.5 μm, thereby forming a primer layer on the PET substrate, and further obtaining a laminate having a pattern portion A exhibiting a structural color on the primer layer and a pattern portion B not exhibiting a structural color, a coating layer C on the pattern portion B, and a coating layer D on the pattern portion A.

[0140] [Examples 2 to 6, 8, 11 to 25, 27 to 31] Laminates were produced in the same manner as in Example 1, except that the combinations were changed as shown in Table 5. In Examples 14 to 17, the thicknesses of pattern portion A were adjusted to 3.0, 6.0, 25.8, and 33.1 μm, respectively.

[0141] In Examples 18 to 20, the coating agent containing a non-aqueous resin and the coating agent containing an aqueous resin were adjusted so that the thickness of the coating layer after drying would be the thickness shown in Table 5.

[0142] Example 7 A coating agent containing the resin fine particles shown in Table 5 was applied to the corona-treated surface of Toyobo Ester Film E5100 using a bar coater selected to give a dried thickness of 10.0 μm, and the coating was dried at 50° C. for 1 minute to form pattern portion A. Furthermore, a coating agent containing a non-aqueous resin was applied to a portion of pattern portion A by gravure printing using a selected plate to give a dried thickness of 1.5 μm, to form pattern portion B and coating layer C. Next, a coating agent containing an aqueous resin was applied to pattern portion A and coating layer C selected to give a dried thickness of 1.5 μm using a bar coater selected to give a laminate having a pattern portion A exhibiting structural color and a pattern portion B not exhibiting structural color on a PET substrate, coating layer C on pattern portion B, and coating layer D on pattern portion A.

[0143] Example 9 The primer coating agent shown in Table 5 was applied to the corona-treated surface of Toyobo Ester Film E5100 using a bar coater to a thickness of 3.0 μm after drying, and the resulting layer was dried at 70° C. for 1 minute to form a primer layer. Next, a coating agent containing resin microparticles shown in Table 5 was applied to a portion of the primer layer using a gravure printing plate selected to a thickness of 10.0 μm after drying, to form pattern portion A. Furthermore, on the primer layer where pattern portion A was not formed, a coating agent containing single-structure resin microparticles of Production Example 15 was applied using a gravure printing plate selected to a thickness of 10.0 μm after drying, to form pattern portion B. Next, a coating agent containing an aqueous resin was applied to pattern portions A and B using a bar coater selected to a thickness of 1.5 μm after drying, to form a primer layer on the PET substrate. A laminate was obtained, which further had pattern portion A exhibiting structural color and pattern portion B not exhibiting structural color on the primer layer, with coating layer D on pattern portion A and coating layer C on pattern portion B.

[0144] Example 10 A primer coating agent shown in Table 5 was applied to the corona-treated surface of Toyobo Ester Film E5100 using a bar coater to a thickness of 3.0 μm after drying, and the resulting coating was dried at 70° C. for 1 minute to form a primer layer. Next, a coating agent containing resin microparticles shown in Table 5 was applied to the primer layer using a bar coater to a thickness of 10.0 μm after drying, and the resulting coating was dried at 50° C. for 1 minute to form pattern portion A. Furthermore, MEK (methyl ethyl ketone) was applied to a portion of pattern portion A by gravure printing as a coating agent not containing resin microparticles, and dried to form pattern portion B. A primer layer was formed on the PET substrate, and a laminate was obtained having pattern portion A exhibiting structural color and pattern portion B not exhibiting structural color on the primer layer.

[0145] [Example 26] The primer coating agent shown in Table 5 was applied to the corona-treated surface of Toyobo Ester Film E5100 using a bar coater selected to give a dried thickness of 3.0 μm, and then dried at 70° C. for 1 minute to form a primer layer. Next, a coating agent containing resin fine particles shown in Table 5 was applied to the primer layer using a bar coater selected to give a dried thickness of 10.0 μm, and then dried at 50° C. for 1 minute to form pattern portion A. Furthermore, a coating agent containing a UV monomer and an initiator was applied to a part of pattern portion A by flexographic printing using a selected plate to give a dried thickness of 1.5 μm, and then the coating was applied using a high-pressure mercury lamp at 500 mJ / cm 2 The pattern portion A was irradiated with ultraviolet light of 1000 W at ...

[0146] Comparative Example 1 The primer coating agent shown in Table 6 was applied to the corona-treated surface of Toyobo Ester Film E5100 using a bar coater to a thickness of 3.0 μm after drying, and the resulting coating was dried at 70° C. for 1 minute to form a primer layer. Next, the coating agent containing the resin fine particles shown in Table 6 was applied to the primer layer using a bar coater to a thickness of 10.0 μm after drying, and the resulting coating was dried at 50° C. for 1 minute to form pattern portion A. Furthermore, MEK (methyl ethyl ketone) was applied to the entire surface of pattern portion A using a bar coater and dried at 70° C. for 1 minute to obtain a laminate having a primer layer and pattern portion B on a PET substrate.

[0147] Comparative Example 2 The primer coating agent shown in Table 6 was applied to the corona-treated surface of Toyobo Ester Film E5100 using a bar coater to a thickness of 3.0 μm after drying, and then dried at 70° C. for 1 minute to form a primer layer. Next, a coating agent containing resin fine particles shown in Table 6 was applied to the primer layer using a bar coater to a thickness of 10.0 μm after drying, and then dried at 50° C. for 1 minute to form pattern portion A, thereby forming a primer layer on the PET substrate and obtaining a laminate having pattern portion A exhibiting structural color on the primer layer. Next, a coating agent containing an aqueous resin was applied to pattern portion A using a bar coater to a thickness of 1.5 μm after drying, thereby forming a primer layer on the PET substrate and obtaining a laminate having pattern portion A exhibiting structural color on the primer layer and a coating layer D on pattern portion A.

[0148] Comparative Example 3 A primer coating agent shown in Table 6 was applied to the corona-treated surface of Toyobo Ester Film E5100 using a bar coater to a thickness of 3.0 μm after drying, and the resulting layer was dried at 70° C. for 1 minute to form a primer layer. Next, a coating agent containing resin fine particles shown in Table 6 was applied to the primer layer using a bar coater to a thickness of 10.0 μm after drying, and the resulting layer was dried at 50° C. for 1 minute to form pattern portion A, thereby forming a primer layer on the PET substrate and obtaining a laminate having pattern portion A exhibiting structural color on the primer layer.

[0149] Next, a pattern portion B was formed using a thermal printer (PocketJet PJ-673 manufactured by Brother Industries, Ltd.) equipped with a thermal head, and a primer layer was formed on the PET substrate, thereby obtaining a laminate having a pattern portion A exhibiting a structural color and a pattern portion B not exhibiting a structural color on the primer layer.

[0150] <Evaluation of Laminate> The obtained laminate was evaluated as follows. The results are shown in Tables 5 and 6.

[0151] [Contrast] The diffuse reflectance spectrum of the laminate was measured in the wavelength range of 350 to 2000 nm using a UV-visible-near-infrared spectrophotometer (V-770D, integrating sphere unit ISN-923, manufactured by JASCO Corporation). The reflectance at each wavelength is the relative reflectance measured using a standard white board with known reflectance (SRS-99-010, manufactured by Labsphere) as a reference. For all laminates, the diffuse reflectance spectra were measured for pattern portion A and pattern portion B from the coated side (assuming a front-side printing configuration) and from the uncoated side (assuming a back-side printing configuration). For the obtained reflectance spectra, the difference (ΔR) between the maximum reflectance due to the structural color and the baseline reflectance not due to the structural color was calculated, and the difference between ΔR in pattern portion A and ΔR in pattern portion B on the coated side and the uncoated side, respectively, was evaluated as contrast, and the best result was adopted.

[0152] In Examples 10 and 11, the contrast evaluation results of the coated side were used, and in Examples 1 to 9 and 12 to 31, the evaluation results of the uncoated side were used.

[0153] (Evaluation criteria) S: Contrast is 70% or more (very good) A: Contrast is 60% or more but less than 70% (good) B: Contrast is 5% or more but less than 60% (usable) C: Contrast is less than 5% or pattern portion A showing structural color is not present (unusable)

[0154] [Gloss] The gloss values ​​of pattern portion A and pattern portion B of the laminate were measured from the coated side using a Micro-TRI-glossmeter manufactured by BYK-Gardner at an incident angle of 60° and an acceptance angle of 60°. (Evaluation criteria) S: The sum of the gloss values ​​of pattern portion A and pattern portion B is 50 or more (very good) A: The sum of the gloss values ​​of pattern portion A and pattern portion B is 40 or more and less than 50 (good) B: The sum of the gloss values ​​of pattern portion A and pattern portion B is 30 or more and less than 40 (usable) C: The sum of the gloss values ​​of pattern portion A and pattern portion B is less than 30 (unusable)

[0155] [Rubbing Resistance] The rubbing resistance of the coated surface of the patterned portion A and patterned portion B of the laminate was measured using a Gakushin-type rubbing fastness tester manufactured by Tester Sangyo Co., Ltd. The measurement conditions were as follows: test piece width 20 mm, load 200 g, 10 reciprocating strokes, against Kanakin No. 3.

[0156] (Evaluation criteria) A: No change in appearance of either pattern portion A or pattern portion B (good) B: Either pattern portion A or pattern portion B is whitened (usable) C: The entire surface of the laminate is whitened (unusable)

[0157]

[0158]

[0159]

[0160]

[0161] From the above results, Comparative Example 1 had poor contrast because the entire surface changed to pattern part B and did not essentially have pattern part A; Comparative Example 2 had poor contrast and abrasion resistance because it did not have pattern part B; and Comparative Example 3 had poor gloss because the resin microparticles in pattern part B were regularly arranged.

[0162] On the other hand, the example had good contrast, gloss and abrasion resistance because it had pattern portion A in which the resin particles were regularly arranged and pattern portion B in which the resin particles were irregularly arranged.

[0163] Although the present invention has been described with reference to the above-mentioned several embodiments, the present invention is not limited to these several embodiments. Various modifications can be made to the configuration and details of the present invention within the scope of the present invention.

[0164] The disclosure of this application is related to the subject matter described in Japanese Patent Application No. 2023-057167, filed on March 31, 2023, the entire disclosure of which is incorporated herein by reference.

Claims

1. A laminate having a pattern portion A that exhibits structural color and a pattern portion B that does not exhibit structural color on a substrate, wherein resin microparticles are regularly arranged in said pattern portion A and resin microparticles are irregularly arranged in said pattern portion B.

2. The laminate according to claim 1, wherein the film thickness of pattern portion A is 5 to 30 μm.

3. A laminate according to claim 1 or 2, in which, when the diffuse reflectance spectrum of pattern portion A is measured at an incident angle of 5°, it exhibits a reflection peak having a half-width of less than 100 nm and a reflected light intensity of 5% or more in the wavelength range of 380 nm to 2000 nm.

4. A laminate according to claim 1 or 2, in which, when the diffuse reflectance spectrum of pattern portion B is measured at an incident angle of 5°, it does not exhibit a reflection peak having a half-width of less than 100 nm and a reflected light intensity of 5% or more in the wavelength range of 380 nm to 2000 nm.

5. The laminate according to claim 1 or 2, further comprising a coating layer on pattern portion A and / or pattern portion B.

6. The laminate according to claim 5, wherein the coating layer has a thickness of 0.1 to 10 μm.

7. The laminate of claim 5, wherein the coating layer comprises a colorant.

8. The laminate according to claim 5, having a coating layer C containing a resin on the pattern portion B.

9. The laminate according to claim 5, having a coating layer D containing a resin on the pattern portion A.

10. The laminate of claim 8, wherein coating layer C comprises a non-aqueous resin.

11. The laminate according to claim 9, wherein coating layer D comprises a water-based resin.

12. A laminate according to claim 1 or 2, having a coating layer C containing a non-aqueous resin on the pattern portion B, and a coating layer D containing an aqueous resin on the pattern portion A.

13. A method for manufacturing a laminate having a pattern portion A that exhibits structural color and a pattern portion B that does not exhibit structural color on a substrate, comprising: step 1 of applying a coating agent containing resin microparticles onto the substrate to form pattern portion A that exhibits structural color due to a regular arrangement of the resin microparticles; and step 2 of applying a coating agent that does not contain resin microparticles to a portion of pattern portion A, thereby changing pattern portion A into pattern portion B that does not exhibit structural color.

Citation Information

Patent Citations

  • Colloid material, and determination method of existence of low dielectric-constant solvent using it

    JP2007051944A

  • Colloid crystal structure and method for producing the same

    JP2010271528A

  • Method for manufacturing patterned colloidal crystal film

    JP2011167663A

  • Elastic body material having periodic structure which varies structural color with modulus

    JP2012000994A

  • Laminated body, thermal recording body, and image forming method

    JP2022080205A